Polyurethane-polyurea aqueous dispersion, and preparation method therefor and use thereof

MYPI2026000910A0Undetermined Publication Date: 2025-05-09WANHUA CHEM GRP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2026000910
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-11-09
Filing Date
2024-01-24
Publication Date
2025-05-09

AI Technical Summary

Technical Problem

The existing polyurethane-polyurea aqueous dispersions used in disposable polyurethane gloves have problems in stability, resulting in common defects in glove production such as cracking and pinholes, which affect the pass rate and thus restrict industrialization.

Method used

By designing specific polyurethane-polyurea aqueous dispersions, polyurethane-polyurea containing terminal carboxyl groups, sulfonate groups and carboxylate groups are used to control the molecular weight between 60,000 and 390,000 yuan, and components such as hydrophilic compounds and polyamines are used to optimize the reaction conditions to improve the stability of the dispersion.

Benefits of technology

The low defects and high stability of the polyurethane-polyurea aqueous dispersion are achieved, ensuring that there is no cracking or pinholes during the production process of gloves, greatly improving the pass rate, and suitable for industrial production.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

Disclosed are a polyurethane-polyurea aqueous dispersion, and a preparation method therefor and a use thereof. The aqueous dispersion comprises a polyurethane-polyurea dispersed therein, containing a terminal carboxyl group, a sulfonate group, and a carboxylate group, and having a specific theoretical molecular weight, wherein the content of the carboxylate group is 1.49-11.9 mmol / 100 g, the content of the sulfonate group is 0.26-7.9 mmol / 100 g, the content of the terminal carboxyl group is 0.5-3.7 mmol / 100 g, the molecular weight is 60,000-390,000, and the specific theoretical molecular weight is a theoretical design molecular weight and is obtained by means of an end-group calculation method. The polyurethane-polyurea aqueous dispersion avoids the problems of glove cracking and pinholes in glove production and improves production stability. No Figure
Need to check novelty before this filing date? Find Prior Art

Description

Polyurethane-polyurea aqueous dispersion and its preparation method and application Technical Field

[0001] The invention belongs to the field of polyurethane-polyurea dispersions, and particularly relates to a polyurethane-polyurea aqueous dispersion and a preparation method and application thereof. Background Art

[0002] Currently, there is little research on polyurethane polyurea aqueous dispersions used in disposable polyurethane gloves, and no industrialized finished gloves have been seen on the market. Research has found that the difficulty lies in the stability of the dispersion, which affects the qualification rate of the gloves. The stability of the dispersion is a key factor affecting glove production.

[0003] Most of the existing solutions focus on the basic physical properties of polyurethane gloves and do not involve issues such as the pass rate, which is precisely the key factor restricting whether the gloves can be industrialized.

[0004] There is an urgent need to solve the problem of qualified rate in this field and eliminate defects such as cracks, pinholes, etc. in gloves produced in order to improve the qualified rate in mass production.

[0005] Summary of the Invention

[0006] One of the purposes of the present invention is to provide a polyurethane-polyurea aqueous dispersion. The inventors have conducted research on the type, content, and molecular weight design of ionic groups that affect flocculation, and have provided a low-defect dispersion that can be stably produced industrially. This ensures that the product will not crack or pinhole during production, greatly improving the pass rate.

[0007] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:

[0008] A polyurethane-polyurea aqueous dispersion comprises a polyurethane-polyurea having a specific theoretical molecular weight and containing terminal carboxyl groups, sulfonate groups, and carboxylate groups, wherein the polyurethane-polyurea has a carboxylate group content of 1.49-11.9 mmol / 100 g, a sulfonate group content of 0.26-7.9 mmol / 100 g, a terminal carboxyl group content of 0.5-3.7 mmol / 100 g, and a molecular weight of 60,000-390,000. The specific theoretical molecular weight is a theoretical design molecular weight obtained by an end group calculation method.

[0009] In one embodiment of the present invention, the dispersion is prepared by reacting raw materials comprising the following components:

[0010] Component a: macromolecular polyol;

[0011] Component b: polyisocyanate;

[0012] Component c: a hydrophilic compound comprising component c1 and component c2; wherein c1 contains 2-3 hydroxyl groups reactive with NCO, and the hydrophilic group is a carboxyl group; c2 contains 2-3 amino groups reactive with NCO, and the hydrophilic group is a salt group;

[0013] Optional component d: small molecule alcohol chain extender;

[0014] Component e: a compound that ionizes the latent groups in component c;

[0015] Component f: a polyamine having a number average molecular weight not exceeding 500 g / mol;

[0016] Component g: a mono-reactive functional compound containing a carboxyl group and an amino group that can react with isocyanate.

[0017] In one embodiment of the present invention, the ratio of the components of the dispersion is:

[0018] Component a: 65-90 parts, preferably 74-88 parts;

[0019] Component b: 8-25 parts, preferably 10-20 parts;

[0020] Component c: 1-6 parts, preferably 1.5-4.8 parts;

[0021] Component d: 0-4 parts, preferably 0-3 parts;

[0022] Component e: 0.1-5 parts, preferably 0.1-3 parts;

[0023] Component f: 0-6 parts, preferably 0-3 parts;

[0024] Component g: 0.05-1 part, preferably 0.085-0.6 part. The ratio of each component is based on mass.

[0025] In the present invention, a monofunctional compound (g) containing carboxyl groups is reacted with isocyanate to produce a polyurethane segment containing terminal carboxyl groups. The introduction of the monofunctional compound can control the molecular weight of the product within a suitable range, avoiding production defects in gloves due to inappropriate molecular weight. Furthermore, the terminal carboxyl groups are more reactive than those in the chain. When this dispersion is used to prepare gloves and other products, the terminal carboxyl groups in the dispersion react more efficiently with the etherified amino resin used as the glove matrix resin, significantly increasing the degree of crosslinking and preventing the mechanical properties of the gloves from being compromised by the end-capping.

[0026] In the polyurethane-polyurea dispersion provided by the present invention, through the mixed use of hydrophilic groups, a suitable content of carboxylate ions improves sensitivity to electrolytes, and a suitable content of sulfonate ions has weaker electrolyte sensitivity than carboxylate ions, which can balance the electrolyte sensitivity of the emulsion, thereby reducing the phenomenon of slagging and skinning during the glove preparation process. The molecular weight of the polyurethane is controlled within a suitable range, so that the wet film formed by the instant demulsification of the glue will not crack due to large molecular weight and cohesive energy and large volume shrinkage, nor will it decline due to insufficient strength due to low molecular weight, thereby avoiding problems such as cracking and glue slippage.

[0027] In one embodiment of the present invention, the component a is one or more of diols, triols and tetraols having a number average molecular weight of 500-6000 g / mol; preferably one or more of polyester polyols, polyether polyols, polycarbonate polyols and polycaprolactone polyols having a number average molecular weight of 500-5000 g / mol and a functionality of 2-3.

[0028] In one embodiment of the present invention, the component b is one or more of aromatic, aliphatic and alicyclic polyisocyanates, preferably one or more of aromatic, aliphatic and alicyclic polyisocyanates having at least two isocyanate groups.

[0029] The component b preferably has the molecular formula Y(NCO)2, wherein Y represents a divalent aliphatic hydrocarbon group containing 4 to 12 carbon atoms, a divalent alicyclic hydrocarbon group containing 6 to 15 carbon atoms, a divalent aromatic hydrocarbon group containing 6 to 15 carbon atoms, or a divalent aromatic aliphatic hydrocarbon group containing 7 to 15 carbon atoms. Suitable diisocyanates may be tetramethylene diisocyanate, methylpentamethylene diisocyanate, hexamethylene diisocyanate, dodecamethylene diisocyanate, 1,4-cyclohexane diisocyanate, isophorone diisocyanate, 4,4′-dicyclohexylmethane diisocyanate, 4,4′-dicyclohexylpropane diisocyanate, 1,4-phenylene diisocyanate, 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, 4,4′-diphenylmethane diisocyanate, 2,2′- and 2,4′-diphenylmethane diisocyanate, tetramethylxylylene diisocyanate, p-xylylene diisocyanate, p-isopropylidene diisocyanate and mixtures of these compounds.

[0030] Component b may also contain small amounts of higher-functionality polyisocyanates known per se in polyurethane chemistry or modified polyisocyanates containing, for example, carbodiimide groups, allophanate groups, isocyanurate groups, urethane groups, and / or biuret groups. Preference is given to hexamethylene diisocyanate, isophorone diisocyanate, dicyclohexylmethane diisocyanate, diphenylmethane diisocyanate, and toluene diisocyanate.

[0031] In one embodiment of the present invention, in the component c, c1 is dimethylolpropionic acid and / or dimethylolbutanoic acid, and c2 is sodium ethylenediaminoethylsulfonate and / or sodium ethylenediaminopropionate.

[0032] In one embodiment of the present invention, the component d is selected from one or more of ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,3-butanediol, 2,3-butanediol, 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, 1,4-dihydroxycyclohexane, 1,4-dihydroxymethylcyclohexane, 1,8-octanediol, 1,10-decanediol, 1,12-dodecanediol, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol and 2-ethyl-1,3-hexanediol; preferably one or more of 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,3-butanediol, neopentyl glycol and 1,4-cyclohexanedimethanol.

[0033] In one embodiment of the present invention, the component e is an organic base, preferably one or more of triethylamine, dimethylethanolamine, and aqueous ammonia, more preferably triethylamine.

[0034] In one embodiment of the present invention, the component f is a polyamine having a number average molecular weight of 60 to 500 g / mol, preferably one or more of ethylenediamine, 1,2-diaminopropane, 1,4-diaminobutane, 1,6-hexanediamine, 2-methyl-1,5-diamine, isophoronediamine, 4,4-diaminodicyclohexylmethane, piperazine and diethylenetriamine, more preferably ethylenediamine and / or isophoronediamine.

[0035] In one embodiment of the present invention, the carboxyl group in the component g can react with the etherified amino resin, and the compound is alkaline. Preferably, component g is a basic amino acid, such as histidine or phenylalanine, more preferably phenylalanine.

[0036] Another object of the present invention is to provide a method for preparing a polyurethane-polyurea aqueous dispersion.

[0037] A method for preparing the above-mentioned polyurethane-polyurea aqueous dispersion, the preparation method comprising the following steps:

[0038] S1: Component a, component b, component c1, optional component d, and a solvent are placed in a reactor and reacted until the NCO content approaches or reaches the theoretical value to obtain an isocyanate-terminated prepolymer;

[0039] S2: Cool down and add solvent to dilute;

[0040] S3: adding component f and component c2 to react, adding component e to neutralize, adding component g to react, adding water to disperse to obtain a dispersion, and removing the solvent to obtain a solvent-free polyurethane-polyurea aqueous dispersion.

[0041] In one embodiment of the present invention, the components in the preparation method are:

[0042] Component a: macromolecular polyol;

[0043] Component b: polyisocyanate;

[0044] Component c: a hydrophilic compound comprising component c1 and component c2; wherein c1 contains 2-3 hydroxyl groups reactive with NCO, and the hydrophilic group is a carboxyl group; c2 contains 2-3 amino groups reactive with NCO, and the hydrophilic group is a salt group;

[0045] Optional component d: small molecule alcohol chain extender;

[0046] Component e: a compound that ionizes the latent groups in component c;

[0047] Component f: a polyamine having a number average molecular weight not exceeding 500 g / mol;

[0048] Component g: a mono-reactive functional compound containing a carboxyl group and an amino group that can react with isocyanate.

[0049] In one embodiment of the present invention, the ratio of each component in the preparation method is:

[0050] Component a: 65-90 parts, preferably 74-88 parts;

[0051] Component b: 8-25 parts, preferably 10-20 parts;

[0052] Component c: 1-6 parts, preferably 1.5-4.8 parts;

[0053] Component d: 0-4 parts, preferably 0-3 parts;

[0054] Component e: 0.1-5 parts, preferably 0.1-3 parts;

[0055] Component f: 0-6 parts, preferably 0-3 parts;

[0056] Component g: 0.05-1 part, preferably 0.085-0.6 part.

[0057] In one embodiment of the present invention, the reaction temperature in S1 is 60-80°C.

[0058] In one embodiment of the present invention, the solvent in S1 is acetone.

[0059] In one embodiment of the present invention, the temperature of the temperature-raising reaction in S2 is 40-45°C.

[0060] In one embodiment of the present invention, the solvent in S2 is acetone.

[0061] In one embodiment of the present invention, component g in S3 is added after component c1 in the polyurethane is neutralized by component e and after the reaction of component c2 is completed.

[0062] In one embodiment of the present invention, the temperature of the temperature-raising reaction in S3 is 40-45°C;

[0063] In one embodiment of the present invention, the solvent in S3 is acetone.

[0064] In one embodiment of the present invention, the solid content of the dispersion obtained in S3 is not less than 35 wt %.

[0065] Compared with the prior art, S3 adds component g after the neutralizer component e is consumed. The purpose is not to increase the hydrophilicity of the chain segment through neutralization, but to control the molecular weight through the monoamino group. At the same time, the presence of the carboxyl group can cross-link with the etherified amino resin in the subsequent preparation of gloves, and the acidity of the carboxyl group can catalyze the cross-linking reaction.

[0066] Another object of the present invention is to provide a use of the polyurethane-polyurea aqueous dispersion.

[0067] A use of a polyurethane-polyurea aqueous dispersion, wherein the dispersion is the above dispersion or a dispersion prepared by the above preparation method, and the use comprises preparing gloves and / or condoms.

[0068] Another object of the present invention is to provide a soft elastic product.

[0069] A soft elastic product is prepared by using the above dispersion or the dispersion prepared by the above preparation method, and the soft elastic product comprises gloves and / or condoms.

[0070] Compared with the prior art, the technical solution provided by the present invention has the following beneficial effects:

[0071] The polyurethane-polyurea dispersion provided by the present invention utilizes a mixture of hydrophilic groups. Carboxylate ions provide electrolyte sensitivity, while sulfonate ions have weaker electrolyte sensitivity than carboxylate ions, balancing the electrolyte sensitivity of the emulsion. This reduces slagging and skinning during glove preparation, and controls the molecular weight of the polyurethane within a suitable range. This ensures that the wet film formed by instant demulsification of the adhesive does not crack due to large molecular weight and cohesive energy, resulting in large volume shrinkage, nor does it decline due to insufficient strength caused by low molecular weight, thereby avoiding problems such as cracking and adhesive slippage. DETAILED DESCRIPTION

[0072] In order to facilitate the understanding of the present invention, the present invention will be further described below in conjunction with examples. It should be understood that the following examples are only for a better understanding of the present invention and do not mean that the present invention is limited to the following examples.

[0073] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which the present invention pertains. The term "and / or" as may be used herein includes any and all combinations of one or more of the associated listed items.

[0074] Where specific experimental steps or conditions are not specified in the examples, the corresponding conventional experimental steps or conditions in the art can be used. Reagents or instruments used without specifying the manufacturer are all commercially available conventional products.

[0075] Hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), toluene diisocyanate (TDI), Wanhua Chemical;

[0076] Polyester polyol 1: poly(adipate-neopentyl glycol) polyester, Mn=2000, Wanhua Chemical;

[0077] Polyester polyol 2: poly(1,4-butanediol-adipate-isophthalate) polyester, Mn=2000, Wanhua Chemical;

[0078] Polyester polyol 3: poly(2-methyl-1,3-propylene glycol adipate), Mn=2000, Wanhua Chemical;

[0079] Polyester polyol 4: polycarbonate polyol (initiators are 1,6-hexanediol and 1,5-pentanediol) Mn=2000, Asahi Kasei Co., Ltd., Japan;

[0080] Polyester polyol 5: polyadipic acid-neopentyl glycol-hexanediol polyester, Mn=1500, Wanhua Chemical;

[0081] Polyether polyol 1: polyoxypropylene glycol, Mn=2000, functionality 2, Wanhua Chemical;

[0082] Polyether polyol 2: polytetramethylene glycol, Mn=2000, functionality 2, Mitsubishi Chemical, Japan;

[0083] Dimethylolpropionic acid (DMPA): Perstorp;

[0084] Sodium ethylenediamine sulfonate (50 wt%), neopentyl glycol (NPG), isophorone diamine (IPDA): Wanhua Chemical;

[0085] Triethylamine (TEA), phenylalanine, histidine, and ethanolamine: Sinopharm Chemical Reagent Co., Ltd.

[0086] pH value: measured using a Metrohm 6173 pH meter.

[0087] Average particle size: The polyurethane dispersion was diluted with water to a concentration of 0.5 wt % and measured using a Malvern Nano-ZS90.

[0088] -NCO determination: The -NCO content during polyurethane synthesis was determined according to the chemical industry standard of the People's Republic of China, "HG / T2409-92 Determination of Isocyanate Group Content in Polyurethane Prepolymers." An NCO tester from Metrohm (Switzerland) was used.

[0089] The specific theoretical molecular weight is the theoretical design molecular weight, which is obtained according to the NCO end group calculation method. The calculation formula is: theoretical design molecular weight = 8400 / blocked NCO %.

[0090] Example 1

[0091] 400 g of polyester polyol 1, 78 g of IPDI, 7.0 g of DMPA, and 152 g of acetone were added to a 1 L four-necked round-bottom flask equipped with a nitrogen inlet and outlet. The mixture was stirred at 80°C until the NCO content reached 1.2 wt% (theoretical value: 1.2 wt%). The mixture was cooled to 45°C and diluted with 600 g of acetone while maintaining the temperature at 43°C. A mixture of 5 g of sodium ethylenediamine sulfonate (50 wt%) and 6 g of IPDA diluted in water was then added with mechanical stirring. The mixture was allowed to react for 15 minutes. 6.0 g of triethylamine was added for neutralization for 5 minutes. Then, 2.5 g of phenylalanine diluted 30 times the amount at 80°C in water was added and the reaction continued for 5 minutes. The mixture was then dispersed in 950 g of deionized water with high-speed stirring at 1000 rpm for 15 minutes. After removing the acetone by vacuum distillation at 55°C and 0.09 MPa, a solvent-free dispersion was obtained. The dispersion had a solids content of 35 wt%, an average particle size of 103 nm, and a pH of 8.1. The theoretical design molecular weight was 65,000. The terminal carboxyl group content was 2.9 mmol / 100 g, the carboxylate group content was 11.8 mmol / 100 g, and the sulfonate group content was 2.6 mmol / 100 g.

[0092] Example 2

[0093] 450g of polyester polyol 2, 78g of IPDI, 4.0g of DMPA, and 152g of acetone were added to a 1L four-necked round-bottom flask equipped with a nitrogen inlet and outlet. The mixture was stirred at 78°C until the NCO content reached 1.18 wt% (theoretical value: 1.18 wt%). The mixture was cooled to 44°C and diluted with 730g of acetone, maintaining the temperature at 44°C. A mixture of 8g of sodium ethylenediamine sulfonate (50 wt%) and 5g of IPDA diluted in water was then added with mechanical stirring. The mixture was allowed to react for 15 minutes, neutralized with 3.0g of triethylamine for 5 minutes, and then 0.8g of phenylalanine diluted 30 times the amount in 80°C water was added, and the reaction continued for 5 minutes. Then, 1098g of deionized water was added with high-speed stirring at 1000 rpm and dispersed for 15 minutes. After removing the acetone by vacuum distillation at 55°C and 0.09 MPa, a solvent-free dispersion was obtained. The dispersion had a solids content of 35 wt%, an average particle size of 173 nm, and a pH of 8.5. The theoretical design molecular weight was 223,000. The terminal carboxyl group content was 0.87 mmol / 100 g, the carboxylate group content was 5.4 mmol / 100 g, and the sulfonate group content was 3.8 mmol / 100 g.

[0094] Example 3

[0095] 450 g of polyester polyol 3, 45 g of HDI, 42 g of IPDI, 2.0 g of DMBA, 8 g of NPG, and 170 g of acetone were added to a 1 L four-necked round-bottom flask equipped with a nitrogen inlet and outlet. The mixture was stirred at 75°C until the NCO content reached 1.64 wt% (theoretical value: 1.64%). The mixture was cooled to 43°C and diluted with 700 g of acetone while maintaining the temperature at 45°C. A mixture of 15 g of sodium ethylenediamine ethylsulfonate (50 wt%) and 5 g of IPDA diluted in water was then added with mechanical stirring. The mixture was allowed to react for 15 minutes, followed by neutralization with 1.2 g of triethylamine for 5 minutes. Then, 1.5 g of phenylalanine diluted 30 times the amount in 80°C water was added and the reaction continued for 5 minutes. The mixture was then stirred at 1000 rpm and then 1130 g of deionized water was added for dispersion for 15 minutes. After removing the acetone by vacuum distillation at 55°C and 0.09 MPa, a solvent-free dispersion was obtained. The dispersion had a solids content of 37 wt%, an average particle size of 115 nm, and a pH of 8.3. The theoretical design molecular weight was 123,000. The terminal carboxyl group content was 1.59 mmol / 100 g, the carboxylate group content was 2.62 mmol / 100 g, and the sulfonate group content was 3.69 mmol / 100 g.

[0096] Example 4

[0097] 560 g of polyester polyol 4, 45 g of HDI, 48 g of IPDI, 15 g of DMPA, and 185 g of acetone were added to a 1 L four-necked round-bottom flask equipped with a nitrogen inlet and outlet. The mixture was stirred at 80° C. until the NCO content reached 0.9 wt % (theoretical value 0.9%). The mixture was cooled to 45° C. and diluted with 700 g of acetone while maintaining the temperature at 43° C. Then, 5 g of sodium ethylenediamine ethylsulfonate (50 wt % content) diluted in water was added with mechanical stirring. The mixture was allowed to react for 15 min. 5.66 g of triethylamine was then added for neutralization for 5 min. Then, 1.0 g of histidine diluted 30 times the amount in 80° C. water was added and the mixture was allowed to react for a further 5 min. Then, 1330 g of deionized water was added with high-speed stirring at 1000 rpm for dispersion for 15 min. After removing the acetone by vacuum distillation at 55°C and 0.09 MPa, a solvent-free dispersion was obtained. The dispersion had a solids content of 35 wt%, an average particle size of 90 nm, and a pH of 8.3. The theoretical design molecular weight was 221,000. The terminal carboxyl group content was 0.9 mmol / 100 g, the carboxylate group content was 8.2 mmol / 100 g, and the sulfonate group content was 1.9 mmol / 100 g.

[0098] Example 5

[0099] 300 g of polyether polyol 1, 300 g of polyether polyol 2, 25 g of TDI, 90 g of IPDI, 19 g of DMPA, and 185 g of acetone were added to a 1 L four-necked round-bottom flask equipped with a nitrogen inlet and outlet. The mixture was stirred at 80°C until the NCO content reached 0.97 wt% (theoretical value 0.97%). The mixture was cooled to 45°C and diluted with 700 g of acetone while maintaining the temperature at 43°C. A mixture of 9 g of sodium ethylenediamine ethylsulfonate (50 wt%) and 3 g of IPDA diluted in water was then added with mechanical stirring. The mixture was allowed to react for 15 minutes, followed by neutralization with 7.17 g of triethylamine for 5 minutes. Afterwards, 0.70 g of phenylalanine diluted 30 times the amount at 80°C in water was added and the reaction continued for 5 minutes. Finally, 1530 g of deionized water was added with high-speed stirring at 1000 rpm for 15 minutes. After removing the acetone by vacuum distillation at 55°C and 0.09 MPa, a solvent-free dispersion was obtained. The dispersion had a solids content of 35 wt%, an average particle size of 110 nm, and a pH of 8.7. The theoretical design molecular weight was 350,000. The terminal carboxyl group content was 0.56 mmol / 100 g, the carboxylate group content was 9.4 mmol / 100 g, and the sulfonate group content was 3.1 mmol / 100 g.

[0100] Example 6

[0101] 450g of polyester polyol 5, 25g of TDI, 90g of IPDI, 19g of DMPA, and 185g of acetone were added to a 1L four-necked round-bottom flask equipped with a nitrogen inlet and outlet. The mixture was stirred at 80°C until the NCO content reached 1.14 wt% (theoretical value: 1.14%). The mixture was cooled to 45°C and diluted with 700g of acetone while maintaining the temperature at 43°C. A mixture of 9g of sodium ethylenediamine ethylsulfonate (50 wt%) and 3g of IPDA diluted in water was then added with mechanical stirring. The mixture was allowed to react for 15 minutes, followed by neutralization with 7.17g of triethylamine for 5 minutes. Afterwards, 0.70g of phenylalanine diluted 30 times the amount at 80°C in water was added and the reaction continued for 5 minutes. Finally, 1230g of deionized water was added with high-speed stirring at 1000 rpm for 15 minutes. After removing the acetone by vacuum distillation at 55°C and 0.09 MPa, a solvent-free dispersion was obtained. The dispersion had a solids content of 38 wt%, an average particle size of 100 nm, and a pH of 8.7. The theoretical design molecular weight was 280,000. The terminal carboxyl group content was 0.69 mmol / 100 g, the carboxylate group content was 11.75 mmol / 100 g, and the sulfonate group content was 3.93 mmol / 100 g.

[0102] Comparative Example 1

[0103] Compared with Example 2, the difference is that 0.8 g of phenylalanine is replaced by 0.3 g of ethanolamine which does not contain a carboxyl group in an equal mole.

[0104] The dispersion had a solids content of 35 wt%, an average particle size of 178 nm, a pH of 8.5, a theoretical design molecular weight of 223,000, a terminal carboxyl group content of 0 mmol / 100 g, a carboxylate group content of 5.4 mmol / 100 g, and a sulfonate group content of 3.8 mmol / 100 g.

[0105] Comparative Example 2

[0106] Compared with Example 1, the difference is that component g is added before neutralization.

[0107] 400 g of polyester polyol 1, 78 g of IPDI, 7.0 g of DMPA, and 152 g of acetone were added to a 1 L four-necked round-bottom flask equipped with a nitrogen inlet and outlet. The mixture was stirred at 80°C until the NCO content reached 1.2 wt% (theoretical value: 1.2 wt%). The mixture was cooled to 45°C and diluted with 600 g of acetone while maintaining the temperature at 43°C. A mixture of 5 g of sodium ethylenediamine sulfonate (50 wt%) and 6 g of IPDA diluted in water was then added with mechanical stirring. The mixture was allowed to react for 15 minutes. 2.5 g of phenylalanine diluted 30 times the amount at 80°C in water was added and the reaction continued for 5 minutes. 7.3 g of triethylamine was added for neutralization for 5 minutes. The mixture was then dispersed in 950 g of deionized water with high-speed stirring at 1000 rpm for 15 minutes. After removing the acetone by vacuum distillation at 55°C and 0.09 MPa, a solvent-free dispersion was obtained. The dispersion had a solids content of 35 wt%, an average particle size of 109 nm, and a pH of 8.2. The theoretical design molecular weight was 65,000. The terminal carboxyl group content was 0.42 mmol / 100 g, the carboxylate group content was 14.28 mmol / 100 g, and the sulfonate group content was 2.6 mmol / 100 g.

[0108] Preparation of glove base resin (liquid): The dispersion prepared above was diluted with deionized water to a solid content of 15 wt%, based on the mass of the diluted dispersion. Then, 0.5 wt% of color paste, 5 wt% of titanium dioxide, and 1.5% of methyl etherified amino resin were added. The mixture was stirred at a low speed (250 rpm) for half an hour and set aside.

[0109] Preparation of coagulation liquid: Use deionized water to prepare an aqueous solution containing 10wt% CaCl2 and 5wt% release agent (calcium stearate), stir continuously for 1h, and set aside.

[0110] Preparation of gloves:

[0111] 1) Place the cleaned glove mold in an oven at 100°C for drying.

[0112] 2) Remove the glove mold, cool it to 55°C, immerse it in the coagulation liquid for 8 seconds, remove it, and place it in a 130°C oven to dry.

[0113] 3) Remove the dried glove mold, cool it to 60°C, immerse it in the prepared matrix resin for 8 seconds, remove it and let it sit for 1 minute (pay attention to whether the glove wrist slides down), then immerse it in 50°C deionized water for 1 minute, remove it and bake it in a 130°C oven for 18 minutes.

[0114] 4) After the baking is completed, the glove mold is taken out and immersed in a glove finishing agent. After being taken out and naturally dried, the mold is demoulded to obtain a finished glove.

[0115] Performance testing:

[0116] Cracking: After demoulding, inflate the gloves and observe whether there are straight and cross-shaped cracks.

[0117] Tensile strength test:

[0118] The palm of the glove was cut into a dumbbell shape with a width of 6 mm and a length of 115 mm. The tensile strength was tested on a tensile testing machine using a high-speed rail company tensile tester at a rate of 200 mm / min.

[0119] Alcohol resistance: After the gloves are inflated, spray 55% alcohol on the surface and observe whether there are any solubility cracks between the fingers.

[0120] The performance test results are shown in Table 1.

[0121] As can be seen from the table, the gloves prepared based on the polyurethane-polyurea aqueous dispersion of the present invention have no cracks, a high pass rate and good alcohol resistance.

[0122] It will be readily understood that the above embodiments are merely examples for clarity of description and are not intended to limit the present invention to these examples. Those skilled in the art will readily appreciate that other variations or modifications based on the above description are possible. It is not necessary and impossible to provide an exhaustive list of all possible implementations. Obvious variations or modifications arising therefrom remain within the scope of protection of the present invention.

Claims

1. A polyurethane-polyurea aqueous dispersion, characterized in that: The dispersion contains polyurethane-polyurea with a specific theoretical molecular weight containing terminal carboxyl groups, sulfonate groups and carboxylate groups dispersed therein, wherein the content of the carboxylate groups is 1.49-11.9 mmol / 100 g, the content of the sulfonate groups is 0.26-7.9 mmol / 100 g, the content of the terminal carboxyl groups is 0.5-3.7 mmol / 100 g, and the molecular weight is 60,000-390,000. The specific theoretical molecular weight is a theoretical design molecular weight obtained by an end group calculation method.

2. The dispersion according to claim 1, characterized in that The dispersion is prepared by reacting raw materials comprising the following components: Component a: macromolecular polyol; Component b: polyisocyanate; Component c: a hydrophilic compound, comprising component c1 and component c2; wherein c1 contains 2-3 hydroxyl groups reactive with NCO, and the hydrophilic group is a carboxyl group; c2 contains 2-3 amino groups reactive with NCO, and the hydrophilic group is a salt group; Optional component d: small molecule alcohol chain extender; Component e: a compound that ionizes the latent groups in component c; Component f: a polyamine having a number average molecular weight not exceeding 500 g / mol; Component g: a mono-reactive functional compound containing a carboxyl group and an amino group that can react with isocyanate.

3. The dispersion according to claim 1 or 2, characterized in that The ratio of each component of the dispersion is: Component a: 65-90 parts, preferably 74-88 parts; Component b: 8-25 parts, preferably 10-20 parts; Component c: 1-6 parts, preferably 1.5-4.8 parts; Component d: 0-4 parts, preferably 0-3 parts; Component e: 0.1-5 parts, preferably 0.1-3 parts; Component f: 0-6 parts, preferably 0-3 parts; Component g: 0.05-1 part, preferably 0.085-0.6 part.

4. The dispersion according to any one of claims 1 to 3, characterized in that The component a is one or more of diols, triols and tetraols with a number average molecular weight of 500-6000 g / mol; preferably one or more of polyester polyols, polyether polyols, polycarbonate polyols and polycaprolactone polyols with a number average molecular weight of 500-5000 g / mol and a functionality of 2-3.

5. The dispersion according to any one of claims 1 to 4, characterized in that The component b is one or more of aromatic, aliphatic and alicyclic polyisocyanates, preferably one or more of aromatic, aliphatic and alicyclic polyisocyanates having at least two isocyanate groups.

6. The dispersion according to any one of claims 1 to 5, characterized in that In the component c, c1 is dimethylol propionic acid and / or dimethylol butyric acid, and c2 is sodium ethylenediamine ethyl sulfonate and / or sodium ethylenediamine propionate.

7. The dispersion according to any one of claims 1 to 6, characterized in that The component d is selected from one or more of ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,3-butanediol, 2,3-butanediol, 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, 1,4-dihydroxycyclohexane, 1,4-dimethylolcyclohexane, 1,8-octanediol, 1,10-decanediol, 1,12-dodecanediol, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol and 2-ethyl-1,3-hexanediol; preferably one or more of 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,3-butanediol, neopentyl glycol and 1,4-cyclohexanedimethanol.

8. The dispersion according to any one of claims 1 to 7, characterized in that The component e is an organic base, preferably one or more of triethylamine, dimethylethanolamine, and aqueous ammonia, more preferably triethylamine.

9. The dispersion according to any one of claims 1 to 8, characterized in that The component f is a polyamine having a number average molecular weight of 60-500 g / mol, preferably one or more of ethylenediamine, 1,2-diaminopropane, 1,4-diaminobutane, 1,6-hexanediamine, 2-methyl-1,5-diamine, isophoronediamine, 4,4-diaminodicyclohexylmethane, piperazine and diethylenetriamine, more preferably ethylenediamine and / or isophoronediamine.

10. The dispersion according to any one of claims 1 to 9, characterized in that The carboxyl group in the component g can react with the etherified amino resin, and the compound is alkaline. Preferably, the component g is a basic amino acid, such as histidine or phenylalanine, more preferably phenylalanine.

11. A method for preparing the polyurethane-polyurea aqueous dispersion according to any one of claims 1 to 10, characterized in that: The preparation method comprises the following steps: S1: putting component a, component b, component c1, optional component d and solvent into a reaction kettle, reacting until the NCO content approaches or reaches the theoretical value, to obtain a prepolymer with terminal isocyanate; S2: Cooling down and adding solvent to dilute; S3: adding component f and component c2 to react, adding component e to neutralize, adding component g to react, adding water to disperse to obtain a dispersion, and removing the solvent to obtain a solvent-free polyurethane-polyurea aqueous dispersion.

12. The preparation method according to claim 11, characterized in that: The components in the preparation method are: Component a: macromolecular polyol; Component b: polyisocyanate; Component c: a hydrophilic compound, comprising component c1 and component c2; wherein c1 contains 2-3 hydroxyl groups reactive with NCO, and the hydrophilic group is a carboxyl group; c2 contains 2-3 amino groups reactive with NCO, and the hydrophilic group is a salt group; Optional component d: small molecule alcohol chain extender; Component e: a compound that ionizes the latent groups in component c; Component f: a polyamine having a number average molecular weight not exceeding 500 g / mol; Component g: a mono-reactive functional compound containing a carboxyl group and an amino group that can react with isocyanate.

13. The preparation method according to claim 11 or 12, characterized in that: The ratio of each component in the preparation method is: Component a: 65-90 parts, preferably 74-88 parts; Component b: 8-25 parts, preferably 10-20 parts; Component c: 1-6 parts, preferably 1.5-4.8 parts; Component d: 0-4 parts, preferably 0-3 parts; Component e: 0.1-5 parts, preferably 0.1-3 parts; Component f: 0-6 parts, preferably 0-3 parts; Component g: 0.05-1 part, preferably 0.085-0.6 part.

14. The preparation method according to claim 11, characterized in that: The reaction temperature in S1 is 60-80°C; And / or, the solvent in S1 is acetone.

15. The preparation method according to claim 11, characterized in that: The temperature of the temperature-raising reaction in S2 is 40-45°C; And / or, the solvent in S2 is acetone.

16. The preparation method according to claim 11, characterized in that: Component g in S3 is added after component c1 in the polyurethane is neutralized by component e and after the reaction of component c2 is completed; and / or, the temperature of the temperature-raising reaction in S3 is 40-45° C.; and / or, the solvent in S3 is acetone; And / or, the solid content of the dispersion obtained in S3 is not less than 35 wt %.

17. Use of a polyurethane-polyurea aqueous dispersion, wherein the dispersion is the dispersion according to any one of claims 1 to 10, or the dispersion prepared by the preparation method according to any one of claims 11 to 16, characterized in that: The use comprises the preparation of gloves and / or condoms.

18. A soft elastic product, wherein the soft elastic product is prepared by using the dispersion according to any one of claims 1 to 10, or by using the dispersion prepared by the preparation method according to any one of claims 11 to 16, characterized in that: The soft elastic products include gloves and / or condoms.