Surface-treatment solution for galvanized steel sheet, method of producing galvanized steel sheet with surface-coating layer, and galvanized steel sheet with surface-coating layer

MYPI2026001426A0Undetermined Publication Date: 2025-04-19JFE STEEL CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2026001426
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-10-19
Filing Date
2024-09-12
Publication Date
2025-04-19

AI Technical Summary

Technical Problem

In the prior art, after long-term exposure to human sweat, the surface treatment layer of zinc-based steel plate has severe blackening phenomenon and insufficient long-term sweat resistance.

Method used

A double-layer surface treatment solution is adopted, wherein the first layer of surface treatment solution contains silane coupling agent, tetrahydrosilicate, manganese niacin compound and sodium silicic acid to form a silicon-rich surface layer; the second layer of surface treatment solution contains anionic polyamide and sodium silicic acid to enhance the barrier effect on sweat components.

Benefits of technology

The long-term sweat resistance of zinc-based steel plates is significantly improved and other properties such as thermal discoloration resistance, thermal cracking resistance, corrosion resistance and coating adhesion are maintained.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

Provided is a surface-treatment solution for a galvanized steel sheet that has excellent storage stability and that can be used to produce a galvanized steel sheet with a surface-coating layer that has excellent long-term perspiration resistance and planar part anti-corrosion property. The surface-treatment solution for galvanized steel sheet includes a first surface-treatment solution (X) and a second surface-treatment solution (Y). The first surface-treatment solution (X) contains a silane coupling agent (A) having a glycidyl group, a tetraalkoxysilane (B), a zirconium carbonate compound (C), a sodium silicate (D1), a vanadium compound (E), a molybdic acid compound (F), and water, the contents of which satisfy defined relationships. The second surface-treatment solution (Y) contains a sodium silicate (D2), an anionic polyurethane resin (G), and water, the contents of which satisfy defined relationships.
Need to check novelty before this filing date? Find Prior Art

Description

Surface treatment solution for zinc-based plated steel sheet, method for manufacturing zinc-based plated steel sheet with surface treatment film, and zinc-based plated steel sheet with surface treatment film

[0001] The present invention relates to a surface treatment liquid for a zinc-based plated steel sheet, a method for producing a zinc-based plated steel sheet with a surface treatment film, and a zinc-based plated steel sheet with a surface treatment film.

[0002] Zinc-based plated steel sheets, which have a zinc-based plating layer on the surface of a substrate steel sheet, have excellent corrosion resistance and are therefore used in a variety of applications, such as automobiles, home appliances, office automation equipment, and building materials. It is also known that when the zinc-based plating layer contains aluminum and / or magnesium as components other than zinc, it exhibits better corrosion resistance than a zinc-based plating layer made of zinc.

[0003] However, it has been observed that when a person's hand directly touches the surface of a zinc-based plating layer, the area touched by the hand turns black over time (black discoloration). This is thought to be due to oxidation of the surface of the zinc-based plating layer caused by the adhesion of sweat components, and is known to be particularly likely to occur in zinc-based plating layers containing aluminum and / or magnesium. Therefore, there is a demand for zinc-based plated steel sheets that do not suffer from the black discoloration even when sweat adheres to them, i.e., that have excellent sweat resistance.

[0004] Patent Document 1 describes a method for producing a zinc-based plated steel sheet with a surface treatment film, in which a surface treatment film is formed on the surface of a zinc-based plated steel sheet using a surface treatment liquid for zinc-based plated steel sheet containing a silane coupling agent having a glycidyl group, a tetraalkoxysilane, sodium silicate, a zirconium carbonate compound, an anionic polyurethane resin having a glass transition temperature (Tg) of 80 to 130°C, a vanadium compound, a molybdenum compound, and water, the pH of which is 8.0 to 10.0, and the contents of the respective components satisfy a predetermined relationship. This production method makes it possible to produce a zinc-based plated steel sheet with a surface treatment film that is excellent in all of heat discoloration resistance, heat cracking resistance, flat plate corrosion resistance, corrosion resistance after alkaline degreasing, blackening resistance, water stain resistance, solvent resistance, sweat resistance, and paint adhesion.

[0005] JP 2018-62710 A

[0006] However, when the present inventors studied the zinc-based plated steel sheet with a surface treatment film proposed in Patent Document 1, they found that the long-term sweat resistance (long-term sweat resistance) was insufficient and that there was room for improvement in the long-term sweat resistance.

[0007] In view of the above problems, the present invention aims to provide a surface treatment solution for zinc-based plated steel sheets that can produce zinc-based plated steel sheets with a surface treatment film that are excellent in all of heat discoloration resistance, heat cracking resistance, flat portion corrosion resistance, processed portion corrosion resistance, corrosion resistance after alkaline degreasing, blackening resistance, water stain resistance, solvent resistance, long-term sweat resistance, and paint adhesion, and that has excellent storage stability. Another object of the present invention is to provide a method for producing zinc-based plated steel sheets with a surface treatment film using the surface treatment solution for zinc-based plated steel sheets, and a zinc-based plated steel sheet with a surface treatment film produced by the production method.

[0008] The present inventors conducted extensive research to solve the above-mentioned problems and discovered the following. By forming a surface treatment film with a laminated structure, the penetration of sweat components can be significantly suppressed. Specifically, a first film having film components that satisfy at least conventional properties other than long-term sweat resistance is formed on the surface of a zinc-based plated steel sheet. The first film contains sodium silicate in addition to a silane coupling agent having a glycidyl group, a tetraalkoxysilane, and a zirconium carbonate compound, which promotes the formation of a silicon-enriched layer on the surface layer and improves long-term sweat resistance. Then, a second film having film components specialized for barrier properties against sweat components is formed on the first film. The second film contains an anionic polyurethane resin, which provides high barrier properties against sweat components, and sodium silicate, which provides strong adhesion to the first film having a silicon-enriched layer, thereby significantly improving long-term sweat resistance.

[0009] That is, the gist and configuration of the present invention are as follows.

[0010] [1] A surface treatment liquid for a zinc-based plated steel sheet, comprising a first surface treatment liquid (X) and a second surface treatment liquid (Y), wherein the first surface treatment liquid (X) contains a silane coupling agent (A) having a glycidyl group, a tetraalkoxysilane (B), a zirconium carbonate compound (C), sodium silicate (D1), a vanadium compound (E), a molybdenum acid compound (F), and water, the contents of each component satisfying the following (1) to (6), and the second surface treatment liquid (Y) contains sodium silicate (D2), an anionic polyurethane resin (G), and water, the contents of each component satisfying the following (7) and (8). (1) A surface treatment liquid for a zinc-based plated steel sheet, comprising a first surface treatment liquid (X) and a second surface treatment liquid (Y), wherein the solid content by mass of the silane coupling agent (A) having a glycidyl group (A) is 100% by mass of the silane coupling agent (A) having a glycidyl group, a tetraalkoxysilane (B), a zirconium carbonate compound (C), sodium silicate (D1), a vanadium compound (E), a molybdenum acid compound (F), and water, the contents of each component satisfying the following (1) to (6). S ) the solid content mass of the silane coupling agent (A) having a glycidyl group (A S ), the solid content mass of tetraalkoxysilane (B) (B S ), and ZrO in the zirconium carbonate compound (C) 2 Converted mass (C Z ) total mass (X S ) to the mass ratio (A S / X S ) is 0.050 to 0.450 (2) The solid content mass of tetraalkoxysilane (B) (B S ) of the total mass (X S ) to the mass ratio (B S / X S ) is 0.010 to 0.190 (3) ZrO in the zirconium carbonate compound (C) 2 Converted mass (C Z ) of the total mass (X S ) to the mass ratio (C Z / X S ) is 0.460 to 0.910 (4) Solid content mass of sodium silicate (D1) (D1 S ) of the total mass (X S ) to the mass ratio (D1 S / X S ) is 0.040 to 0.630 (5) The V-equivalent mass (E) of the vanadium compound (E) V ) of the total mass (X S ) and the solid content mass of sodium silicate (D1) (D1 S ) and the total mass (XS +D1 S ) to the mass ratio (E V / (X S +D1 S )) is 0.006 to 0.094 (6) Mo-equivalent mass (F) of the molybdenum acid compound (F) M ) of the total mass (X S ) and the solid content mass of sodium silicate (D1) (D1 S ) and the total mass (X S +D1 S ) to the mass ratio (F M / (X S +D1 S )) is 0.030 to 0.280 (7) Solid content mass of sodium silicate (D2) (D2 S ) the solid content mass of the anionic polyurethane resin (G) (G S ) to the mass ratio (D2 S / G S ) is 0.010 to 0.100 (8) The solid content mass (G S ) the solid content mass (Y S ) to the mass ratio (G S / Y S ) is 0.900 to 0.980

[0011] [2] The surface treatment liquid for zinc-based plated steel sheets according to the above [1], wherein in the second surface treatment liquid (Y), the anionic polyurethane resin (G) contains an anionic polyurethane resin having a carbonate skeleton, and the content thereof satisfies the following (9): (9) The solid content mass of the anionic polyurethane resin (G) is 1 / 2 the solid content mass of the anionic polyurethane resin having a carbonate skeleton. S ) mass ratio is 0.20 to 0.80

[0012] [3] The second surface treatment liquid (Y) further contains a silicone resin (H), and the content thereof satisfies the following (10): (10) The solid content by mass of the silicone resin (H) S ) the solid content mass of the anionic polyurethane resin (G) (G S ) to the mass ratio (HS / G S ) is 0.0030 to 0.0400

[0013] [4] The second surface treatment liquid (Y) further contains a crosslinking agent (I), the content of which satisfies the following (11): (11) The solid content by mass of the crosslinking agent (I) S ) the solid content mass of the anionic polyurethane resin (G) (G S ) to the mass ratio (I S / G S ) is 0.0030 to 0.0400

[0014] [5] The second surface treatment solution (Y) for a zinc-based coated steel sheet according to any one of [1] to [4] above, further containing a wax (L), the content of which satisfies the following (12): (12) The solid content by mass of the wax (L) S ) the solid content mass (Y S ) to the mass ratio (L S / Y S ) is 0.010 to 0.120

[0015] [6] The surface treatment solution for zinc-based coated steel sheets according to any one of the above [1] to [5], wherein the first surface treatment solution (X) further contains a phosphate compound (J), and the content thereof satisfies the following (13): (13) The solid content by mass of the phosphate compound (J S ) of the total mass (X S ) to the mass ratio (J S / X S ) is 0.140 to 0.770

[0016] [7] The surface treatment solution for zinc-based coated steel sheets according to any one of the above [1] to [6], wherein the first surface treatment solution (X) further contains a fluorine compound (K), and the content thereof satisfies the following (14): (14) The solid content by mass of the fluorine compound (K) S ) of the total mass (X S ) to the mass ratio (K S / X S ) is 0.040 to 0.610

[0017] [8] A method for producing a zinc-based plated steel sheet having a surface treatment film, using the surface treatment liquid for zinc-based plated steel sheet according to any one of [1] to [7] above, comprising the steps of: applying the first surface treatment liquid (X) to a surface of a zinc-based plated steel sheet; then drying the applied first surface treatment liquid (X) to form a first film; then applying the second surface treatment liquid (Y) to the surface of the first film; and then drying the applied second surface treatment liquid (Y) to form a second film.

[0018] [9] The coating amount of the first coating is 0.010 to 0.400 g / m 2 and the coating amount of the second coating is 0.20 to 3.00 g / m 2 The method for producing a zinc-based plated steel sheet having a surface treatment film according to [8] above,

[0019]

[10] A zinc-based plated steel sheet having a surface treatment film, produced by the method for producing a zinc-based plated steel sheet having a surface treatment film according to [8] or [9] above.

[0020]

[11] The zinc-based plated steel sheet with a surface treatment film according to the above

[10] , wherein the zinc-based plated steel sheet is a hot-dip Zn-Al-based alloy plated steel sheet having, on at least one surface of a base steel sheet as a substrate, a hot-dip Zn-Al-based alloy plating layer having a component composition containing, in mass %, Al: 3.0 to 12.0%, Mg: 0.2 to 6.0%, Ni: 0.0 to 0.1%, and the balance consisting of Zn and unavoidable impurities.

[0021] The present invention can provide a surface treatment solution for zinc-based plated steel sheets that can produce zinc-based plated steel sheets with a surface treatment film that is excellent in all of heat discoloration resistance, heat cracking resistance, flat portion corrosion resistance, processed portion corrosion resistance, corrosion resistance after alkaline degreasing, blackening resistance, water stain resistance, solvent resistance, long-term sweat resistance, and paint adhesion, and that has excellent storage stability. The present invention also can provide a method for producing a zinc-based plated steel sheet with a surface treatment film that uses the surface treatment solution for zinc-based plated steel sheets, and a zinc-based plated steel sheet with a surface treatment film produced by the production method.

[0022] Hereinafter, embodiments of the surface treatment solution for a zinc-based plated steel sheet, the method for producing a zinc-based plated steel sheet with a surface treatment film, and the zinc-based plated steel sheet with a surface treatment film according to the present invention will be described. Note that the embodiment described below is an example of the present invention, and the configuration of the present invention is not limited to this specific example.

[0023] (Surface treatment liquid for zinc-based plated steel sheet) A surface treatment liquid for zinc-based plated steel sheet according to one embodiment of the present invention comprises a first surface treatment liquid (X) and a second surface treatment liquid (Y). The first surface treatment liquid (X) is applied to the surface of a zinc-based plated steel sheet and dried to form a first coating on the zinc-based plated steel sheet. The second surface treatment liquid (Y) is applied to the first coating and dried to form a second coating on the first coating.

[0024] [First surface treatment liquid (X)] The first surface treatment liquid (X) contains a silane coupling agent (A) having a glycidyl group, a tetraalkoxysilane (B), a zirconium carbonate compound (C), sodium silicate (D1), a vanadium compound (E), a molybdic acid compound (F), and water, and may further contain one or both of a phosphate compound (J) and a fluorine compound (K), as necessary.

[0025] <Silane Coupling Agent (A) Having a Glycidyl Group> The first surface treatment liquid (X) contains a silane coupling agent (A) having a glycidyl group. The silane coupling agent (A) is not particularly limited, as long as it is a silane coupling agent in which a glycidyl group and a lower alkoxy group having 1 to 5 carbon atoms, preferably 1 to 3 carbon atoms as a hydrolyzable group, are directly bonded to a Si element. Examples of the silane coupling agent (A) include 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane. Among these, 3-glycidoxypropyltrimethoxysilane and 3-glycidoxypropyltriethoxysilane are preferred, from the viewpoint that they facilitate the generation of more condensation points between silane coupling agents (A) having glycidyl groups themselves, or with a tetraalkoxysilane (B) or a zirconium carbonate compound (C) described below, thereby achieving high barrier properties after film formation.

[0026] The silane coupling agent (A) having a glycidyl group has an alkoxy group directly bonded to the Si element in the compound, and the alkoxy group reacts with water in an aqueous solution to form a silanol group. The silanol group reacts with the surface of the zinc-based plated steel sheet or undergoes a complex condensation reaction with the tetraalkoxysilane (B) and the zirconium carbonate compound (C) described below.

[0027] The solid content mass of the silane coupling agent (A) having a glycidyl group (A S ) the solid content mass of the silane coupling agent (A) having a glycidyl group (A S ), the solid content mass of tetraalkoxysilane (B) (B S ), and ZrO in the zirconium carbonate compound (C) 2 Converted mass (C Z ) total mass (X S ) to the mass ratio (A S / X S The mass ratio (A) is 0.050 to 0.450. S / X SIf the mass ratio (A) is less than 0.050, the corrosion resistance of the flat plate portion, the corrosion resistance of the processed portion, and the corrosion resistance after alkaline degreasing are poor. S / X S ) is 0.050 or more, preferably 0.060 or more, and more preferably 0.090 or more. S / X S If the mass ratio (A) exceeds 0.450, the heat cracking resistance is poor. S / X S ) is 0.450 or less, preferably 0.380 or less, and more preferably 0.290 or less.

[0028] <Tetraalkoxysilane (B)> The first surface treatment liquid (X) contains tetraalkoxysilane (B) because the use of component (A) alone results in poor thermal cracking resistance. Without component (B), the carbon-carbon bonds of component (A) undergo thermal oxidative decomposition in a heated atmosphere of 500°C or higher, resulting in the generation of large cracks. In contrast, adding an appropriate amount of component (B) allows a dense coating with high barrier properties to be obtained while keeping the amount of component (A) added to a level that allows for acceptable thermal cracking resistance. Because the coating obtained from components (A) and (B) is dense, cracks that occur during heating can be minimized, and no cracks visible to the naked eye occur, resulting in excellent thermal cracking resistance.

[0029] Tetraalkoxysilane (B) has four lower alkoxy groups as hydrolyzable groups directly bonded to the Si element, and is represented by the general formula Si(OR) 4 (wherein R is the same or different alkyl group having 1 to 5 carbon atoms) is not particularly limited as long as it is represented by the formula. Examples of the tetraalkoxysilane (B) include tetramethoxysilane, tetraethoxysilane, and tetrapropoxysilane, and one or more of these can be used. Among these, tetraethoxysilane and tetramethoxysilane are preferred from the viewpoint that they are more likely to generate condensation points between tetraalkoxysilanes (B) themselves, or with component (A) and component (C) described below, thereby achieving high barrier properties after film formation.

[0030] Tetraalkoxysilane (B) has an alkoxy group directly bonded to the Si element in the compound, and the alkoxy group reacts with water in an aqueous solution to form a silanol group, which reacts with the surface of the zinc-based plated steel sheet or undergoes a complex condensation reaction with component (A) or component (C) described below.

[0031] Solid mass of tetraalkoxysilane (B) (B S ) of the total mass (X S ) to the mass ratio (B S / X S The mass ratio (B) is set to 0.010 to 0.190. S / X S If the mass ratio (B) is less than 0.010, the corrosion resistance of the flat plate portion, the corrosion resistance of the processed portion, and the corrosion resistance after alkaline degreasing will be reduced. S / X S ) is 0.010 or more, preferably 0.020 or more, and more preferably 0.030 or more. S / X S If the mass ratio (B) exceeds 0.190, the thermal cracking resistance is reduced. S / X S ) is 0.190 or less, preferably 0.150 or less, and more preferably 0.110 or less.

[0032] Although component (A) and component (B) may be used alone, it is preferable to subject component (A) and component (B) to a condensation reaction to form a low condensation product, which is then added to the first surface treatment liquid (X), thereby obtaining higher barrier properties after film formation. This low condensation product has a polysiloxane bond as its main skeleton formed by a condensation reaction between the silanol groups of component (A) and component (B), and all of the terminal groups bonded to the Si element may be alkoxy groups, or some of the groups directly bonded to the Si element may be alkoxy groups.

[0033] The low condensation product obtained by the condensation reaction of component (A) and component (B) preferably has a condensation degree of 2 to 30, more preferably 2 to 10. A condensation degree of 30 or less allows for stable use of component (A) and component (B) in aqueous solution without forming a white precipitate. This low condensation product can be obtained by reacting component (A), component (B), and a chelating agent described below at a reaction temperature of 1 to 70°C for approximately 10 minutes to 20 hours, followed by autoclaving. Examples of chelating agents include hydroxycarboxylic acids such as malic acid, acetic acid, and tartaric acid; monocarboxylic acids; polycarboxylic acids such as dicarboxylic acids or tricarboxylic acids, including oxalic acid, malonic acid, succinic acid, citric acid, and adipic acid; and aminocarboxylic acids such as glycine. One or more of these can be used.

[0034] The condensation state of this low condensate can be measured by gel permeation chromatography (GPC), NMR, and FT-IR as described in JIS-K7252-4.

[0035] The chelating agent that stabilizes this low condensate acts when the alkoxy groups of component (A) and component (B) undergo a hydrolysis reaction with water and the chelating agent. The stabilizing effect of the chelating agent is thought to be achieved by the chelating agent appropriately coordinating with the silanol groups derived from components (A) and (B) generated by the hydrolysis reaction, although the reason for this is unclear. That is, the moderate coordination of the chelating agent with the silanol groups suppresses excessive condensation of components (A) and (B), resulting in a first surface treatment liquid (X) with excellent storage stability. Furthermore, the first coating can maintain stable quality even after long-term storage of the first surface treatment liquid (X).

[0036] The chelating agent is effective not only in ensuring storage stability but also in ensuring the corrosion resistance of the first coating. Although the reason for this is unclear, it is thought that the chelating agent also coordinates with the vanadium compound (E), which will be described later. When the first coating is exposed to a corrosive environment, the chelating agent coordinated to the vanadium compound (E) is eluted together with the vanadium compound (E). This promotes condensation of component (A) and component (B), which have lost their ligands, within the first coating, thereby further enhancing the barrier properties of the first coating and contributing to improved corrosion resistance.

[0037] <Zirconium carbonate compound (C)> The first surface treatment liquid (X) contains a zirconium carbonate compound (C). When the first surface treatment liquid (X) contains a zirconium carbonate compound (C), a first coating that is difficult to dissolve in water is obtained, thereby improving the corrosion resistance and water stain resistance of the flat plate portion. Furthermore, by using the zirconium carbonate compound (C) in combination with sodium silicate (D1) described below, a first coating that is particularly excellent in long-term sweat resistance can be obtained.

[0038] The first coating containing the above components (A) to (C) normally exhibits moderate hardness and flexibility, high barrier properties, and excellent corrosion resistance in flat portions, processed portions, and after alkaline degreasing. The high barrier properties are due to the presence of hydroxyl groups in the zirconium carbonate compound (C), which serve as condensation points with silanol groups. Furthermore, since the zirconium carbonate compound (C) produces zirconium oxide and zirconium hydroxide upon drying, the dense coating of the tetraalkoxysilane (B) and the zirconium carbonate compound (C) prevents visually noticeable cracks even when heated above 500°C, providing excellent thermal cracking resistance. Examples of the zirconium carbonate compound (C) include salts of zirconium carbonate, such as sodium, potassium, lithium, and ammonium. One or more of these salts may be used. Among these, ammonium zirconium carbonate and potassium zirconium carbonate are preferred in terms of film-forming properties and water stain resistance.

[0039] ZrO in zirconium carbonate compound (C) 2 Converted mass (C Z ) of the total mass (X S ) to the mass ratio (C Z / X S The mass ratio (C Z / X S When the mass ratio (C) is less than 0.460, the barrier property derived from the zirconium carbonate compound (C) is insufficient, and the corrosion resistance after alkaline degreasing is reduced. Z / X S ) is 0.460 or more, preferably 0.580 or more, and more preferably 0.630 or more. Z / X S If the mass ratio (C) exceeds 0.910, the amount of hard components derived from the zirconium carbonate compound is large, and good coating adhesion cannot be obtained. Z / X S ) is 0.910 or less, preferably 0.900 or less, and more preferably 0.870 or less.

[0040] <Sodium silicate (D1)> The first surface treatment liquid (X) contains sodium silicate (D1). Sodium contained in the sodium silicate (D1) is converted to SiO 4 SiO separated from the interconnected network 4 It bonds to the tetrahedral oxygen atoms. 4 The recombination of the interconnecting network is prevented. This action imparts fluidity to the silicate glass, lowering the softening temperature of the silicate glass from 1700°C or higher to 500°C to 700°C. In the present invention, this action is utilized to impart fluidity to the first coating, which is hard and has a low thermal expansion coefficient and contains components (A) to (C), when heated to 500°C or higher, thereby achieving excellent thermal cracking resistance.

[0041] The sodium silicate (D1) used in the present invention is a highly water-soluble component, but also has the ability to etch zinc. Therefore, when the first surface treatment liquid (X) comes into contact with the surface of the zinc-based plating layer and dries, zinc ions dissolved in the first surface treatment liquid (X) are fixed as sparingly soluble metal silicate salts, contributing to the adhesion of the first coating. Furthermore, the inventors discovered that when sodium silicate (D1) is contained in the first surface treatment liquid (X) in combination with components (A) to (C), the formation of a silicon-enriched layer on the surface of the first coating is promoted. Furthermore, the inventors discovered that the presence of this silicon-enriched layer improves long-term sweat resistance. This is believed to be due to the condensation of the silanol groups of the sodium silicate (D1), the silane coupling agent (A), the silanol groups of the tetraalkoxysilane (B), and the hydroxyl groups of the zirconium carbonate compound (C), which incorporates the sodium silicate (D1), forming a denser network. Furthermore, in a corrosive environment, the sodium silicate (D1) immobilized in the first coating as described above is appropriately eluted, and this action of manipulating the pH of the surface of the zinc-based plating layer toward the alkaline side also contributes to delaying and inhibiting the anodic reaction of zinc.

[0042] The sodium silicate (D1) used in the present invention is SiO 2 and Na 2 O, and the molar ratio thereof is SiO 2 / Na 2 It is preferable that O is 1 to 4. SiO 2 / Na 2 By setting the O content to 4 or less, the effect on thermal cracking resistance can be suitably obtained. 2 / Na 2 By making O 1 or more, the sodium silicate (D1) can be suitably fixed in the first coating film while ensuring the effect on thermal cracking resistance, and deterioration of blackening resistance, water stain resistance, and long-term sweat resistance can be suitably suppressed. 2 / Na 2 O is preferably 1 or more, more preferably 2 or more. Examples of the sodium silicate (D1) that satisfies the above include sodium silicate No. 2 and sodium silicate No. 3, and one or more of these can be used.

[0043] Solid content mass of sodium silicate (D1) (D1 S ) of the total mass (X S ) to the mass ratio (D1 S / X S The mass ratio (D1 S / X S When the mass ratio (D1 S / X S ) is 0.040 or more, and preferably 0.050 or more. S / X S If the mass ratio (D1) exceeds 0.630, sodium silicate becomes excessive, making it difficult to fix it in the first coating, resulting in poor blackening resistance, water stain resistance, and long-term sweat resistance. Furthermore, since a large amount of Na ions will be present in the first surface treatment liquid (X), the storage stability of the first surface treatment liquid (X) will be reduced. Therefore, S / X S ) is 0.630 or less, preferably 0.470 or less.

[0044] <Vanadium Compound (E)> The first surface treatment liquid (X) contains a vanadium compound (E). The vanadium compound (E) is uniformly dispersed in the first coating, but moderately dissolves in a corrosive environment. The vanadium compound (E) bonds with the zinc ions dissolved in the corrosive environment to form a dense passive coating, thereby improving the corrosion resistance of the flat plate portion, the corrosion resistance of the processed portion, and the corrosion resistance after alkaline degreasing. Examples of the vanadium compound (E) include ammonium metavanadate, sodium metavanadate, vanadium acetylacetonate, and metavanadyl acetylacetonate, and one or more of these can be used.

[0045] The V-equivalent mass (E) of the vanadium compound (E) V ) of the total mass (X S ) and the solid content mass of sodium silicate (D1) (D1 S ) and the total mass (X S +D1 S ) to the mass ratio (E V / (XS +D1 S The mass ratio (E V / (X S +D1 S If the mass ratio (E ) is less than 0.006, the effect of forming a passive film with zinc ions is insufficient, and therefore the corrosion resistance of the flat plate portion, the corrosion resistance of the processed portion, and the corrosion resistance after alkaline degreasing are reduced. V / (X S +D1 S )) is 0.006 or more, preferably 0.008 or more, and more preferably 0.012 or more. V / (X S +D1 S If the mass ratio (E ) exceeds 0.094, good blackening resistance and water stain resistance cannot be obtained. Furthermore, when heated to above 500°C, oxidation discoloration of vanadium occurs, and the heat discoloration resistance also decreases. Therefore, V / (X S +D1 S )) is 0.094 or less, preferably 0.071 or less, and more preferably 0.047 or less.

[0046] <Molybdic Acid Compound (F)> The first surface treatment liquid (X) contains a molybdic acid compound (F). By containing the molybdic acid compound (F), blackening resistance is improved. Examples of the molybdic acid compound (F) include molybdic acid, ammonium molybdate, sodium molybdate, potassium molybdate, magnesium molybdate, and zinc molybdate. In the present invention, it is preferable to use one or more compounds selected from these.

[0047] The blackening phenomenon of zinc-based plating layers is thought to be due to the formation of oxygen-deficient zinc oxide when the zinc-based plating layer is exposed to a high-temperature, high-humidity atmosphere. Molybdenum is a second transition metal with various valences, and in air it combines with oxygen to form MoO 2 or MoO 3 In the present invention, MoO 4 2- This molybdate is added uniformly to the first coating, and then heated in a high-temperature, high-humidity atmosphere to form MoO 3It is believed that molybdenum is reduced to molybdenum oxides such as molybdenum oxides of the formula (I) and molybdenum oxides of the formula (II). This action provides an appropriate supply of oxygen to the zinc on the surface of the zinc-based coating layer, which is believed to suppress the formation of oxygen-deficient zinc oxide. On the other hand, if an excessive amount of molybdate is added, the corrosion resistance of flat parts, processed parts, and corrosion resistance after alkaline degreasing cannot be obtained.

[0048] Mo-equivalent mass (F) of the molybdic acid compound (F) M ) of the total mass (X S ) and the solid content mass of sodium silicate (D1) (D1 S ) and the total mass (X S +D1 S ) to the mass ratio (F M / (X S +D1 S The mass ratio (F M / (X S +D1 S If the mass ratio (F M / (X S +D1 S )) is 0.030 or more, preferably 0.040 or more, and more preferably 0.050 or more. M / (X S +D1 S If the mass ratio (F ) exceeds 0.280, good corrosion resistance of the flat plate portion, corrosion resistance of the processed portion, and corrosion resistance after alkaline degreasing cannot be obtained. M / (X S +D1 S )) is 0.280 or less, preferably 0.240 or less, and more preferably 0.190 or less.

[0049] <Phosphate Compound (J)> The first surface treatment solution (X) may contain a phosphate compound (J) for the purpose of further improving the corrosion resistance of the first coating. The phosphate compound (J) dissolves appropriately in a corrosive environment, bonds with the zinc ions dissolved in the corrosive environment, and forms a sparingly soluble zinc phosphate coating film, which covers coating defects and thereby improves the corrosion resistance of the flat plate portion, the corrosion resistance of the processed portion, and the corrosion resistance after alkaline degreasing.

[0050] The phosphoric acid compound (J) can be at least one selected from inorganic phosphoric acid compounds and organic phosphoric acid compounds. Examples of inorganic phosphoric acid compounds include phosphoric acid, primary phosphates, secondary phosphates, and tertiary phosphates; condensed phosphates such as pyrophosphoric acid, pyrophosphate, tripolyphosphoric acid, and tripolyphosphate; phosphorous acid, phosphites, hypophosphorous acid, and hypophosphites. Examples of organic phosphoric acid compounds include phosphonic acid, diphosphonic acid, phosphonobutanetricarboxylic acid, ethylenediaminetetramylenephosphonic acid, methyldiphosphonic acid, methylenephosphonic acid, ethylidenediphosphonic acid, and ammonium salts and alkali metal salts thereof. For flaky plating peeling resistance, inorganic phosphoric acid compounds such as phosphoric acid or ammonium dihydrogen phosphate are preferred because they more easily form sparingly soluble metal salts. When using organic phosphoric acid compounds, diphosphonic acid is preferred because it provides better water stain resistance and storage stability of the first surface treatment liquid (X).

[0051] Solid mass of phosphoric acid compound (J) S ) of the total mass (X S ) to the mass ratio (J S / X S The mass ratio (J) is preferably 0.140 to 0.770. S / X S By making the mass ratio (J) 0.140 or more, the corrosion resistance of the flat plate portion, the corrosion resistance of the processed portion, and the corrosion resistance after alkaline degreasing can be suitably obtained. S / X S ) is preferably 0.140 or more, more preferably 0.180 or more, and even more preferably 0.280 or more. S / X S By making the mass ratio (J) 0.770 or less, heat discoloration resistance, blackening resistance, water stain resistance, long-term sweat resistance, and paint adhesion can be suitably obtained. S / X S ) is preferably 0.770 or less, more preferably 0.720 or less, and even more preferably 0.660 or less.

[0052] <Fluorine Compound (K)> The first surface treatment solution (X) may contain a fluorine compound (K) for the purpose of further improving adhesion between the first coating and the surface of the zinc-based plated steel sheet. The fluorine compound (K) slightly etches the zinc-based plated surface, forming fine irregularities on the surface of the zinc-based plated layer, thereby improving adhesion through an anchoring effect.

[0053] From the viewpoint of suppressing excessive dissolution of the plating, examples of the fluorine compound (K) include hydrofluoric acid, hydrosilicofluoric acid, ammonium fluoride, lithium fluoride, sodium fluoride, potassium fluoride, ammonium acid fluoride, sodium acid fluoride, potassium acid fluoride, fluorotitanic acid, ammonium fluorotitanate, fluorozirconic acid, and ammonium fluorozirconate, and in the present invention, it is preferable to use one or more compounds selected from these.

[0054] Solid mass of fluorine compound (K) (K S ) of the total mass (X S ) to the mass ratio (K S / X S The mass ratio (K) is preferably 0.040 to 0.610. S / X S By making the mass ratio (K) 0.040 or more, it is possible to obtain favorable long-term sweat resistance and coating adhesion. S / X S ) is preferably 0.040 or more, more preferably 0.050 or more, and even more preferably 0.080 or more. S / X S By making the mass ratio (K) 0.610 or less, the corrosion resistance of the flat plate portion, the corrosion resistance of the processed portion, the corrosion resistance after alkaline degreasing, the blackening resistance, and the water stain resistance can be suitably obtained. S / X S ) is preferably 0.610 or less, more preferably 0.450 or less, and even more preferably 0.300 or less.

[0055] <pH of 8.0 to 10.0> The first surface treatment liquid (X) can be obtained by mixing the above-mentioned components in water such as deionized water or distilled water. The solids content of the first surface treatment liquid (X) may be selected as appropriate, but is preferably 5 to 20% by mass. The pH of the first surface treatment liquid (X) is preferably 8.0 to 10.0. When the pH of the first surface treatment liquid (X) is 8.0 or higher, the storage stability of the first surface treatment liquid (X) can be favorably achieved. Therefore, the pH of the first surface treatment liquid (X) is preferably 8.0 or higher, and more preferably 8.5 or higher. On the other hand, when the pH of the first surface treatment liquid (X) is 10.0 or lower, the storage stability of the first surface treatment liquid (X) can be favorably achieved, and further, etching of the zinc-based plating layer is favorable, and corrosion resistance of the flat plate portion, corrosion resistance of the processed portion, and corrosion resistance after alkaline degreasing can be favorably achieved. Therefore, the pH of the first surface treatment liquid (X) is preferably 10.0 or less, and more preferably 9.5 or less. When adjusting the pH, ammonia or a salt thereof, and one or more of the chelating agents described above may be appropriately used.

[0056] Furthermore, additives such as alcohols, ketones, cellosolves, amine-based water-soluble solvents, antifoaming agents, antibacterial and antifungal agents, colorants, wettability improvers for uniform coating, resins, surfactants, etc. may be added to the first surface treatment liquid (X) as needed. However, it is important to add these additives in amounts that do not impair the quality obtained by the present invention, and the amount added is preferably less than 5 mass % at most based on the total solid content of the first surface treatment liquid (X).

[0057] Furthermore, the first surface treatment liquid (X) may contain a trace amount of at least one of the anionic polyurethane resin (G), silicone resin (H), crosslinking agent (I), and wax (L) contained in the second surface treatment liquid (Y) described below. In this case, the quality obtained by the present invention is not impaired as long as the total mass of the solid contents thereof is 30 mass% or less relative to the total solid content of the first surface treatment liquid (X). Therefore, when the first surface treatment liquid (X) contains one or more of the anionic polyurethane resin (G), silicone resin (H), crosslinking agent (I), and wax (L), the total mass of the solid contents thereof is preferably 30 mass% or less, more preferably 20 mass% or less, even more preferably 10 mass% or less, and most preferably 5 mass% or less relative to the total solid content of the first surface treatment liquid (X).

[0058] [Second surface treatment liquid (Y)] The second surface treatment liquid (Y) contains sodium silicate (D2), an anionic polyurethane resin (G), and water, and may further contain, as necessary, one or more components selected from the group consisting of a silicone resin (H), a crosslinking agent (I), and a wax (L).

[0059] <Sodium silicate (D2)> The second surface treatment liquid (Y) contains sodium silicate (D2). The silanol groups contained in sodium silicate (D2) strengthen the adhesion of the second coating to the first coating, contributing to long-term sweat resistance. Furthermore, when used in combination with the anionic polyurethane resin (G) described below, the high cohesiveness of the urethane bonds in the anionic polyurethane resin (G) allows sodium silicate (D2) to be incorporated into a dense, highly barrier polyurethane resin coating. In a corrosive environment, the sodium silicate (D2) immobilized in the second coating as described above moderately dissolves, and by manipulating the pH of the surface of the zinc-based plating layer toward the alkaline side, it also contributes to delaying and suppressing the anodic reaction of zinc.

[0060] The sodium silicate (D2) used in the present invention is SiO 2 and Na 2 O, and the molar ratio thereof is SiO 2 / Na 2 It is preferable that O is 1 to 4. SiO 2 / Na 2By setting the O content to 4 or less, the effect on thermal cracking resistance can be suitably obtained. 2 / Na 2 By making the O content 1 or more, the sodium silicate (D2) can be suitably fixed in the second coating film while ensuring the effect on thermal cracking resistance, and the deterioration of blackening resistance, water stain resistance, and long-term sweat resistance can be suitably suppressed. 2 / Na 2 O is preferably 1 or more, more preferably 2 or more. Examples of the sodium silicate (D2) that satisfies the above conditions include sodium silicate No. 2 and sodium silicate No. 3, and one or more of these can be used.

[0061] The sodium silicate (D1) blended in the first surface treatment liquid (X) and the sodium silicate (D2) blended in the second surface treatment liquid (Y) may be the same or different. Since laminating films having different constituent components is effective in effectively improving long-term sweat resistance, it is preferable that the sodium silicate (D1) blended in the first surface treatment liquid (X) and the sodium silicate (D2) blended in the second surface treatment liquid (Y) are different.

[0062] Solid content mass of sodium silicate (D2) (D2 S ) the solid content mass of the anionic polyurethane resin (G) (G S ) to the mass ratio (D2 S / G S ) is 0.010 to 0.100. Mass ratio (D2 S / G S If the mass ratio (D2 S / G S On the other hand, the mass ratio (D2 S / G S If the mass ratio (D2) exceeds 0.100, the sodium silicate (D2) will be in excess, making it difficult to fix it in the second coating, resulting in poor blackening resistance, water stain resistance, and long-term sweat resistance. Furthermore, the second surface treatment liquid (Y) will contain a large amount of Na ions, which will reduce the storage stability of the second surface treatment liquid (Y). Therefore,S / G S ) is 0.100 or less, preferably 0.070 or less, and more preferably 0.050 or less.

[0063] <Anionic polyurethane resin (G)> The second surface treatment liquid (Y) contains an anionic polyurethane resin (G) that has excellent barrier properties against sweat components. This makes the second coating denser, contributing to improved long-term sweat resistance. Polyurethane resins have a high molecular weight and urethane bonds with strong intermolecular cohesive force, making them dense and providing excellent barrier properties. They also have high adhesion to the first coating, making it possible to obtain a second coating with the above-mentioned excellent performance.

[0064] Examples of types of polyols, which are the basic skeleton that determines the properties of urethane resins, include polyether polyols, polyester polyols, and polycarbonate polyols. Polyester polyols and polycarbonate polyols have polar groups, which allow for intermolecular interactions to form a tough second coating. Polycarbonate polyols are expensive but have excellent mechanical strength. Polyether polyols do not have polar groups, which means they are somewhat inferior in mechanical strength, but are chemically stable, such as in terms of hydrolysis resistance. Anionic polyurethane resins (G) can be used alone or in combination of two or more types, in the second surface treatment liquid (Y).

[0065] The weight-average molecular weight of the anionic polyurethane resin (G) is not particularly limited, but is preferably about 5,000 to 500,000, and more preferably about 10,000 to 300,000, as measured by gel permeation chromatography as described in JIS-K7252-4. Increasing the weight-average molecular weight can increase the Tg and mechanical properties of the urethane resin, thereby improving the barrier properties of the second coating and further enhancing flat plate corrosion resistance, corrosion resistance after alkaline degreasing, water stain resistance, long-term sweat resistance, solvent resistance, and the like.

[0066] The anionic polyurethane resin (G) is obtained by a general synthesis method using a polyol such as polyester polyol, polyether polyol, or polycarbonate polyol and a polyisocyanate as raw materials. Although not intended to be limiting, a more specific synthesis method involves, for example, producing a urethane prepolymer having isocyanato groups at both ends from a polyol and a polyisocyanate, reacting this with a carboxylic acid having two hydroxyl groups or a reactive derivative thereof in a solvent to obtain a derivative having isocyanato groups at both ends, and then adding triethanolamine or the like as a counter cation, followed by adding the resulting mixture to water to form an emulsion, thereby obtaining an anionic polyurethane resin. If necessary, a diamine may then be added to carry out chain extension.

[0067] The polyisocyanate used in producing the anionic polyurethane resin (G) includes aliphatic, alicyclic and aromatic polyisocyanates, and any of them can be used. Specific examples include tetramethylene diisocyanate, hexamethylene diisocyanate, lysine diisocyanate, hydrogenated xylylene diisocyanate, 1,4-cyclohexylene diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, 2,4'-dicyclohexylmethane diisocyanate, isophorone diisocyanate, 3,3'-dimethoxy-4,4'-biphenylene diisocyanate, 1,5-naphthalene diisocyanate, 1,5-tetrahydronaphthalene diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, phenylene diisocyanate, xylylene diisocyanate, and tetramethylxylylene diisocyanate. Among these, the use of aliphatic or alicyclic polyisocyanates such as tetramethylene diisocyanate, hexamethylene diisocyanate, lysine diisocyanate, hydrogenated xylene diisocyanate, 1,4-cyclohexylene diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, 2,4'-dicyclohexylmethane diisocyanate, and isophorone diisocyanate is preferred because it provides a second coating that is excellent not only in flat plate corrosion resistance, corrosion resistance after alkaline degreasing, and solvent resistance, but also in heat discoloration resistance.

[0068] Examples of polyester polyols used in producing the anionic polyurethane resin (G) include various polyester polyols obtained by a dehydration condensation reaction between a glycol or triol, such as ethylene glycol, diethylene glycol, or trimethylolpropane, and a dibasic acid, such as adipic acid or phthalic anhydride; and lactone-based polyester polyols obtained by ring-opening polymerization of ε-caprolactam.

[0069] Examples of polyether polyols used in producing the anionic polyurethane resin (G) include low molecular weight polyols such as 1,2-propanediol, 1,3-propanediol, trimethylolpropane, glycerin, polyglycerin, and pentaerythritol, as well as ethylene oxide and / or propylene oxide adducts of amine compounds such as bisphenol A and ethylenediamine, and polytetramethylene ether glycol.

[0070] Examples of polycarbonate polyols used in producing the anionic polyurethane resin (G) include those obtained by reacting glycols such as ethylene glycol, diethylene glycol, propylene glycol, dipropylene glycol, neopentyl glycol, methylpentanediol, dimethylbutanediol, butylethylpropanediol, diethylene glycol, triethylene glycol, tetraethylene glycol, 1,4-butanediol, 1,4-cyclohexanediol, and 1,6-hexanediol with diphenyl carbonate, phosgene, or the like.

[0071] The carboxylic acid or its reactive derivative having two or more, preferably two, hydroxyl groups used in producing the anionic polyurethane resin (G) is used to introduce acidic groups into component (G) and to make component (G) water-dispersible. Examples of the carboxylic acid include dimethylolalkanoic acids such as dimethylolpropionic acid, dimethylolbutanoic acid, dimethylolpentanoic acid, and dimethylolhexanoic acid. Examples of reactive derivatives include acid anhydrides. By making component (G) self-water-dispersible in this way and using as little or no emulsifier as possible, a second coating with excellent water stain resistance can be obtained.

[0072] A polyamine, water, or the like is used when producing the anionic polyurethane resin (G). This polyamine, water, or the like is used to extend the chain of the prepared prepolymer. Examples of polyamines used in producing the anionic polyurethane resin (G) include hydrazine, ethylenediamine, propylenediamine, 1,6-hexanediamine, tetramethylenediamine, isophoronediamine, xylylenediamine, piperazine, 1,1'-bicyclohexane-4,4'-diamine, diphenylmethanediamine, ethyltolylenediamine, diethylenetriamine, dipropylenetriamine, triethylenetetramine, and tetraethylenepentamine, and these can be used alone or in combination.

[0073] In order to improve the stability of the anionic polyurethane resin (G) during synthesis and to enhance film-forming properties in a low-temperature, dry environment during film formation, it is preferable to incorporate a film-forming aid during synthesis. Examples of the film-forming aid include butyl cellosolve, N-methyl-2-pyrrolidone, butyl carbitol, and Texanol, with N-methyl-2-pyrrolidone being preferred.

[0074] The glass transition point (Tg) of the anionic polyurethane resin (G) is preferably 30 to 130°C. A glass transition point (Tg) of 30°C or higher can suppress a decrease in the barrier properties of the second coating and achieve sufficient solvent resistance. Therefore, the glass transition point (Tg) of the anionic polyurethane resin (G) is preferably 30°C or higher, and more preferably 50°C or higher. On the other hand, a glass transition point (Tg) of the anionic polyurethane resin (G) of 130°C or lower can prevent the second coating from becoming excessively hard and is less likely to crack during processing, resulting in excellent paint adhesion. Therefore, the glass transition point (Tg) of the anionic polyurethane resin (G) is preferably 130°C or lower, and more preferably 110°C or lower. The glass transition point can be adjusted by, for example, the molecular weight of the polyol used.

[0075] The glass transition point (Tg) of the anionic polyurethane resin (G) can be determined from the maximum value of tan δ by measuring the dynamic viscoelasticity using a dynamic viscoelasticity measuring device (RSAG2, TA Instrument) and using a film prepared by drying at room temperature for 24 hours, then at 80°C for 6 hours and then at 120°C for 20 minutes as a measurement sample.

[0076] Solid mass of anionic polyurethane resin (G) (G S ) the solid content mass of the second surface treatment liquid (Y) (Y S ) to the mass ratio (G S / Y S The mass ratio (G S / Y S If the mass ratio (G) is less than 0.900, the amount of the anionic polyurethane resin (G) is small, resulting in poor long-term sweat resistance, and also poor resistance to blackening and water stains. S / Y S ) is 0.900 or more, preferably 0.930 or more, and more preferably 0.950 or more. S / Y S If the mass ratio (G) exceeds 0.980, the amount of sodium silicate (D2) decreases relatively, which reduces the adhesion between the second coating and the first coating, and also reduces the corrosion resistance of the processed portion and the corrosion resistance after alkaline degreasing. S / Y S ) shall be 0.980 or less.

[0077] In the second surface treatment liquid (Y), the anionic polyurethane resin (G) preferably contains an anionic polyurethane resin having a carbonate skeleton. Due to the high cohesive strength of the carbonate bonds, anionic polyurethane resins having a carbonate skeleton have small gaps in the resin, resulting in excellent barrier properties that inhibit the permeation of sweat components or corrosive factors, and are also less susceptible to hydrolysis. Therefore, a second coating is obtained that is resistant to deterioration in high-temperature, high-humidity environments and can maintain excellent long-term sweat resistance and corrosion resistance for a long period of time. In particular, from the perspective of improving long-term sweat resistance, it is preferable to combine a polyether-based polyol and a polycarbonate-based polyol as the anionic polyurethane resin (G).

[0078] The solid content mass of the anionic polyurethane resin (G) having a carbonate skeleton is S ) is preferably 0.20 to 0.80. By setting the mass ratio to 0.20 or more, long-term sweat resistance can be suitably obtained. Therefore, the mass ratio is preferably 0.20 or more, and more preferably 0.30 or more. On the other hand, by setting the mass ratio to 0.80 or less, solvent resistance can be suitably obtained. Therefore, the mass ratio is preferably 0.80 or less, and more preferably 0.70 or less.

[0079] <Silicone Resin (H)> The second surface treatment liquid (Y) may further contain a silicone resin (H). This allows for the production of a second coating with superior water stain resistance and long-term sweat resistance. The silicone resin (H) is not particularly limited as long as it has a plurality of siloxane bonds and an organopolysiloxane structure in which an organic group is bonded to silicon (Si). However, an organopolysiloxane structure having at least two organic groups bonded to Si per molecule is preferred. The position at which the organic group is bonded is not particularly limited, and it may be bonded to the main chain, side chain, or terminal. The silicone resin (H) may be a homopolymer having the above-mentioned organopolysiloxane structure, a mixture of a homopolymer having the above-mentioned organopolysiloxane structure and a homopolymer having a polysiloxane structure, or a copolymer (block copolymer or graft polymer) having the above-mentioned organopolysiloxane structure and a polysiloxane structure. The silicone resin (H) may be of either an addition type or a condensation type. Furthermore, the silicone resin (H) may be any of a heat-curing type, a room temperature curing type (RTV) and a UV-curing type.

[0080] Solid mass of silicone resin (H) S ) the solid content mass of the anionic polyurethane resin (G) (G S ) to the mass ratio (H S / G S The mass ratio (H S / G SBy making the mass ratio (H ) 0.0030 or more, excellent water repellency and oil repellency can be obtained, and the effects of improving water stain resistance and long-term sweat resistance can be suitably obtained. S / G S ) is preferably 0.0030 or more, more preferably 0.0040 or more. S / G S By making the mass ratio (H S / G S ) is preferably 0.0400 or less, more preferably 0.0320 or less.

[0081] <Crosslinking Agent (I)> The second surface treatment liquid (Y) may contain a crosslinking agent (I) that reacts with carboxyl groups in order to further improve the corrosion resistance of the processed portion of the second coating. The anionic polyurethane resin (G) contains carboxyl groups in the second coating, and the crosslinking agent (I) crosslinks with these groups to modify the organic components of the second coating. In other words, a second coating with high barrier properties and flexibility is formed, and cracking of the second coating is suppressed even when bending is performed, thereby improving the corrosion resistance of the bent portion. The crosslinking agent (I) is preferably a compound having two or more functional groups capable of reacting with carboxyl groups per molecule. Examples of functional groups capable of reacting with carboxyl groups include epoxy groups, carbodiimide groups, and oxazoline groups. Examples of the crosslinking agent (I) include epoxy resins, carbodiimide resins, and oxazoline group-containing polymers, and it is preferable to use one or more selected from these.

[0082] Solid mass of crosslinking agent (I) (I S ) the solid content mass of the anionic polyurethane resin (G) (G S ) to the mass ratio (I S / G S The mass ratio (I) is preferably 0.0030 to 0.0400. S / G S By making the mass ratio (I) 0.0030 or more, the effect of improving the corrosion resistance and solvent resistance of the processed part can be suitably obtained. S / G S) is preferably 0.0030 or more, more preferably 0.0040 or more. S / G S By making the mass ratio (I) 0.0400 or less, the corrosion resistance of the flat plate portion, the corrosion resistance of the processed portion, the corrosion resistance after alkaline degreasing, and the solvent resistance can be suitably obtained. S / G S ) is preferably 0.0400 or less, more preferably 0.0320 or less.

[0083] <Wax (L)> The second surface treatment liquid (Y) may contain wax (L) to improve the lubricity of the second coating surface. The wax (L) is not particularly limited as long as it is compatible with the second surface treatment liquid (Y), and examples thereof include polyolefin waxes such as polyethylene, montan wax, paraffin wax, microcrystalline wax, carnauba wax, lanolin-based wax, silicone-based wax, and fluorine-based wax, and one or more of these can be suitably used. In addition, examples of polyolefin waxes include polyethylene wax, oxidized polyethylene wax, and polypropylene wax, and one or more of these can be used.

[0084] Solid mass of wax (L) (L S ) the solid content mass of the second surface treatment liquid (Y) (Y S ) to the mass ratio (L S / Y S The mass ratio (L S / Y S By making the mass ratio (L ) 0.010 or more, the effect of improving the lubricity of the surface of the second coating can be suitably obtained. S / Y S ) is preferably 0.010 or more. S / Y S By setting the mass ratio (L) to 0.120 or less, the lubricity is not too high, and it is possible to suitably prevent the coil from being crushed during the winding process in the coil manufacturing process. Furthermore, it is possible to suitably obtain corrosion resistance and paint adhesion in the processed part. Therefore, S / Y S) is preferably 0.120 or less, more preferably 0.090 or less.

[0085] The second surface treatment liquid (Y) can be obtained by mixing the above-mentioned components in water such as deionized water or distilled water. The solid content of the second surface treatment liquid (Y) can be selected appropriately, but is preferably 5 to 20 mass %. The pH of the second surface treatment liquid (Y) is not particularly limited, but is preferably 9.8 to 10.8.

[0086] Furthermore, additives such as alcohols, ketones, cellosolves, amine-based water-soluble solvents, antifoaming agents, antibacterial and antifungal agents, colorants, wettability improvers for uniform coating, resins, surfactants, etc. may be added to the second surface treatment liquid (Y) as needed. However, it is important that these additives are added in amounts that do not impair the quality obtained by the present invention, and the amount added is preferably less than 5 mass % at most based on the total solid content of the second surface treatment liquid (Y).

[0087] (Method for manufacturing a zinc-based plated steel sheet with a surface treatment film) A method for manufacturing a zinc-based plated steel sheet with a surface treatment film according to one embodiment of the present invention is a method for manufacturing a zinc-based plated steel sheet with a surface treatment film using the above-mentioned surface treatment liquid for a zinc-based plated steel sheet, and includes the steps of applying a first surface treatment liquid (X) to the surface of the zinc-based plated steel sheet, then drying the applied first surface treatment liquid (X) to form a first film, then applying a second surface treatment liquid (Y) to the surface of the first film, and then drying the applied second surface treatment liquid (Y) to form a second film. The conditions and methods for forming the first film and the second film are described in detail below.

[0088] Before applying the first surface treatment liquid (X) to the surface of the zinc-based plated steel sheet, the zinc-based plated steel sheet may be subjected to a pretreatment for the purpose of removing oil or dirt from the surface of the zinc-based plated steel sheet, as necessary. The surface of a zinc-based plated steel sheet is often coated with an anti-rust oil for rust prevention purposes, and even if it is not coated with an anti-rust oil, oil or dirt may adhere to the surface during operation. By carrying out the above pretreatment, the surface of the zinc-based plated steel sheet is cleaned and easily wetted uniformly. If the surface of the zinc-based plated steel sheet is free of oil or dirt and can be uniformly wetted with the first surface treatment liquid (X), a pretreatment step is not particularly necessary. The pretreatment method is not particularly limited, and examples thereof include hot water washing, organic solvent washing, and alkaline degreasing washing.

[0089] As a method for applying the first surface treatment liquid (X) to the surface of the zinc-based plated steel sheet and a method for applying the second surface treatment liquid (Y) to the surface of the first coating, an optimum method may be selected depending on the shape of the zinc-based plated steel sheet to be treated, etc. Examples of such methods include roll coating, bar coating, immersion, spray coating, etc. After application, it is also possible to adjust the amount of coating, achieve a uniform appearance, and achieve a uniform film thickness by an air knife method or a roll squeezing method.

[0090] After the first surface treatment solution (X) has been applied to the surface of the zinc-based plated steel sheet, a drying oven such as a hot air oven, a high-frequency induction heating oven, or an infrared oven can be used as a means for drying the applied first surface treatment solution (X).

[0091] The peak metal temperature (PMT) during drying of the first surface treatment solution (X) is preferably 40 to 100°C. By setting the peak metal temperature to 40°C or higher, the condensation reaction of the Si component contained in the first surface treatment solution (X) can be favorably progressed, forming a denser Si-enriched layer. On the other hand, by setting the peak metal temperature to 100°C or lower, cracking of the first coating can be favorably suppressed.

[0092] The heating time when drying the first surface treatment liquid (X) is appropriately selected under optimum conditions depending on the composition of the zinc-based plated steel sheet used, the process and configuration of the production line, etc., and from the viewpoint of productivity, etc., the heating time is preferably from 0.1 to 60 seconds, and more preferably from 1 to 30 seconds.

[0093] The amount of the first coating applied after drying is 0.010 to 0.400 g / m per side. 2 It is preferable that the density is 0.030 to 0.250 g / m 2 It is more preferable that the coating weight of the first coating is 0.010 g / m 2 By setting the coating weight of the first coating to 0.400 g / m or more, barrier properties can be suitably obtained, and the corrosion resistance of the flat plate portion, corrosion resistance after alkaline degreasing, blackening resistance, long-term sweat resistance, and water stain resistance can be suitably obtained. 2 By setting the thickness as follows, the thickness of the first coating is suitable, and suitable resistance to heat discoloration and heat cracking is obtained.

[0094] After the second surface treatment liquid (Y) is applied to the surface of the first coating, a drying oven such as a hot air oven, a high-frequency induction heating oven, or an infrared oven can be used as a means for drying the applied second surface treatment liquid (Y) in addition to a dryer.

[0095] Here, the maximum sheet temperature reached when drying the second surface treatment liquid (Y) is preferably 60 to 200°C, more preferably 80 to 180°C. If the maximum sheet temperature reached is 60°C or higher, bonding between the components of the second coating is obtained, and the various performances required by the present invention are preferably obtained. On the other hand, if the maximum sheet temperature reached is 200°C or lower, cracking of the second coating or thermal decomposition of the coating components is unlikely to occur, and the various performances required by the present invention are preferably obtained.

[0096] The heating time when drying the second surface treatment liquid (Y) is appropriately selected under optimal conditions depending on the composition of the zinc-based plated steel sheet used, the process and configuration of the production line, etc., and from the viewpoint of productivity, etc., the heating time is preferably from 0.1 to 60 seconds, and more preferably from 1 to 30 seconds.

[0097] The amount of the second coating applied after drying is 0.20 to 3.00 g / m per side. 2 It is preferable that the density is 0.40 to 2.00 g / m 2 It is more preferable that the coating weight of the second coating is 0.20 g / m.2 By setting the coating weight of the second coating to 3.00 g / m or more, sufficient barrier properties are obtained, and the corrosion resistance of the flat plate portion, the corrosion resistance after alkaline degreasing, the long-term sweat resistance, and the water stain resistance are preferably obtained. 2 By setting the following, heat discoloration resistance, heat cracking resistance, and paint adhesion can be suitably obtained.

[0098] For steps and conditions not described in the present invention, conventional methods can be used.

[0099] (Zinc-based plated steel sheet with surface treatment film) A zinc-based plated steel sheet with a surface treatment film according to one embodiment of the present invention is a zinc-based plated steel sheet with a surface treatment film manufactured by the manufacturing method described above, and includes a zinc-based plated steel sheet and a surface treatment film formed on at least one side of the zinc-based plated steel sheet.

[0100] [Zinc-based plated steel sheet] The zinc-based plated steel sheet used in the present invention may be an electrogalvanized steel sheet, a hot-dip galvanized steel sheet, a zinc-aluminum alloy plated steel sheet, a zinc-iron alloy plated steel sheet, a zinc-magnesium alloy plated steel sheet, a zinc-aluminum-magnesium alloy plated steel sheet, or the like.

[0101] More preferably, a hot-dip Zn-Al alloy-plated steel sheet can be used, which has a hot-dip Zn-Al alloy plating layer on at least one surface of a substrate steel sheet, the hot-dip Zn-Al alloy plating layer containing, by mass %, 3.0 to 12.0% Al, 0.2 to 6.0% Mg, and 0.0 to 0.1% Ni, with the balance being Zn and unavoidable impurities. Use of this hot-dip Zn-Al alloy-plated steel sheet offers the advantage of superior red rust resistance compared to other plated steel sheets. This makes it advantageous for use in more severe corrosive environments, such as outdoors. While the hot-dip Zn-Al alloy plating layer does not necessarily contain Ni, it is preferable to contain 0.1 mass % or less of Ni, as this provides favorable blackening resistance. More preferably, the hot-dip Zn-Al alloy-plated steel sheet contains a Zn-Al-Mg ternary eutectic in the hot-dip Zn-Al alloy plating layer. The Zn-Al-Mg ternary eutectic is preferably contained in an area ratio of 1 to 50% on the surface of the plating layer.

[0102] [Surface Treatment Film] The surface treatment film of the present invention includes a first film on a zinc-based plated steel sheet and a second film on the first film. The first film is obtained by applying the above-mentioned first surface treatment liquid (X) to the surface of the zinc-based plated steel sheet and drying it. The second film is obtained by applying the above-mentioned second surface treatment liquid (Y) to the surface of the first film and drying it. The zinc-based plated steel sheet with a surface treatment film of this embodiment is excellent in all of heat discoloration resistance, heat cracking resistance, corrosion resistance of flat plate portions, corrosion resistance of processed portions, corrosion resistance after alkaline degreasing, blackening resistance, water stain resistance, solvent resistance, long-term sweat resistance, and paint adhesion.

[0103] It is important that the surface treatment film has a silicon-enriched layer on the outermost surface of the first film and a resin-based second film. During the drying stage of the first film, the Zr component bonds faster than the Si component, forming regions where the Si component is incorporated into the network structure of the Zr component and regions where the Si component is concentrated. The anionic polyurethane resin itself of the second film has high barrier properties against sweat components, and the inclusion of sodium silicate provides strong adhesion to the first film with the silicon-enriched layer, significantly improving long-term sweat resistance.

[0104] The effects of the present invention will be explained below with reference to examples and comparative examples, but these examples are merely examples for explaining the present invention and do not limit the present invention.

[0105] (1) Test Sheets Table 1 shows various zinc-based plated steel sheets used as test sheets. The zinc-based plated layers were formed on both sides of the steel sheet (base steel sheet), and the coating weights in Table 1 refer to the coating weights of the zinc-based plated layers per side.

[0106]

[0107] (2) Pretreatment (Washing) The surface of the above-mentioned test plate was treated with Fine Cleaner E6406 manufactured by Nihon Parkerizing Co., Ltd. to remove oil or dirt from the surface. Next, the test plate was washed with tap water to confirm that the surface of the test plate was 100% wetted with water, and then pure water (deionized water) was poured over the surface, and the water was dried in an oven at 100°C.

[0108] (3) Preparation of Surface Treatment Liquid The components shown in Table 2 were mixed in water at the respective blending ratios (mass ratios) shown in Table 2 to obtain a first surface treatment liquid (X) with a solid content of 6 mass %. The components shown in Table 3 were mixed in water at the respective blending ratios (mass ratios) shown in Table 3 to obtain a second surface treatment liquid (Y) with a solid content of 15 mass %.

[0109] The components shown in Table 4 were mixed in water in the respective blending ratios (mass ratios) shown in Table 4 to obtain first surface treatment liquids X48 to X50 with a solid content of 6 mass %. Note that first surface treatment liquids X48 and X49 are intended to be prepared by incorporating the components contained in the first surface treatment liquid (X) and second surface treatment liquid (Y) of the present invention into a single surface treatment liquid. In particular, X49 has the same composition as the surface treatment liquid disclosed in Patent Document 1. Furthermore, X50 is prepared by incorporating the anionic polyurethane resin (G4) into the first surface treatment liquid X1 in Table 2 at 30 mass % relative to the total solid content of X50. Note that in Table 4, the total mass (X) is calculated in accordance with Patent Document 1. S ) the solid content mass of the anionic polyurethane resin (G) (G S ) to the mass ratio (X S / G S ) is stated.

[0110] The compounds used in Tables 2 to 4 are described below.

[0111] <Silane coupling agent (A) having a glycidyl group> A1: 3-glycidoxypropyltriethoxysilane A2: 3-glycidoxypropyltrimethoxysilane

[0112] <Tetraalkoxysilane (B)> B1: Tetraethoxysilane B2: Tetramethoxysilane

[0113] <Zirconium carbonate compound (C)> C1: ammonium zirconium carbonate (ZrO 2 : 20.0 mass%) C2: potassium zirconium carbonate (ZrO 2 :20.0% by mass)

[0114] <Sodium silicate (D1, D2)> D-1: No. 3 sodium silicate (solid content: 38.5% by mass) D-2: No. 2 sodium silicate (solid content: 40.6% by mass)

[0115] <Vanadium Compound (E)> E1: Metavanadyl acetylacetonate (V: 19.2% by mass) E2: Ammonium metavanadate (V: 43.5% by mass)

[0116] <Molybdic Acid Compounds (F)> F1: Ammonium molybdate (Mo: 54.4% by mass) F2: Sodium molybdate (Mo: 43.8% by mass)

[0117] <Anionic Polyurethane Resin (G)> Method for Producing Anionic Polyurethane Resin (G1) 100 parts by mass of a polyether polyol having a number average molecular weight of 5,000 obtained from polyethylene glycol and polypropylene glycol, 5 parts by mass of 2,2-dimethyl-1,3-propanediol, 100 parts by mass of 4,4-dicyclohexylmethane diisocyanate, 20 parts by mass of 2,2-dimethylolpropionic acid, and 120 parts by mass of N-methyl-2-pyrrolidone were added to a reactor to obtain a urethane prepolymer having a free isocyanato group content of 5% relative to the solids content. Next, 16 parts by mass of tetramethylenediamine and 10 parts by mass of triethylamine were added to 500 parts by mass of deionized water, and the urethane prepolymer was added and emulsified while stirring with a homomixer. Finally, deionized water was added to obtain a water-dispersible anionic polyurethane resin (G1) having a solids content of 25% by mass. In the anionic polyurethane resin (G1), the solid content mass of the anionic polyurethane resin having a carbonate skeleton is S The glass transition temperature (Tg) of the resulting anionic polyurethane resin (G1) was measured using a dynamic viscoelasticity measuring device and was found to be 95°C.

[0118] A water-dispersible anionic polyurethane resin (G2) having a solid content of 25% by mass was obtained in the same manner as in the production method for anionic polyurethane resin (G1), except that 20 parts by mass of 1,4-butanediol-2-sulfonic acid was used in place of 20 parts by mass of 2,2-dimethylolpropionic acid in the reactor. S The glass transition temperature (Tg) of the resulting anionic polyurethane resin (G2) was measured using a dynamic viscoelasticity measuring device and was found to be 95°C.

[0119] Production method for anionic polyurethane resin (G3) A water-dispersible anionic polyurethane resin (G3) having a solids content of 25% by mass was obtained in the same manner as in the production method for anionic polyurethane resin (G1), except that 100 parts by mass of a polyester polyol having a number average molecular weight of 2220 obtained from 1,6-hexanediol and adipic acid was used in place of 100 parts by mass of a polyether polyol having a number average molecular weight of 5000 obtained from polyethylene glycol and polypropylene glycol. In the anionic polyurethane resin (G3), the solids content of the anionic polyurethane resin (G3) was 25% by mass. S The glass transition temperature (Tg) of the resulting anionic polyurethane resin (G3) was measured using a dynamic viscoelasticity measuring device and was found to be 70°C.

[0120]

[0043] A water-dispersible anionic polyurethane resin (G4) having a solids content of 25% by mass was obtained in the same manner as in the production method for anionic polyurethane resin (G1), except that 100 parts by mass of a polyether polyol having a number average molecular weight of 1,560 obtained from polyethylene glycol and polypropylene glycol was used in place of 100 parts by mass of a polyether polyol having a number average molecular weight of 5,000 obtained from polyethylene glycol and polypropylene.

[0044] In the anionic polyurethane resin (G4), the solids content of the anionic polyurethane resin (G4) was 25% by mass. S The glass transition temperature (Tg) of the resulting anionic polyurethane resin (G4) was measured using a dynamic viscoelasticity measuring device and was found to be 105°C.

[0121] Production method for anionic polyurethane resin (G5) A water-dispersible anionic polyurethane resin (G5) having a solids content of 25% by mass was obtained in the same manner as in the production method for anionic polyurethane resin (G1), except that 100 parts by mass of a polyester polyol having a number average molecular weight of 1,320 obtained from 1,6-hexanediol and adipic acid was used in place of 100 parts by mass of a polyether polyol having a number average molecular weight of 5,000 obtained from polyethylene glycol and polypropylene glycol. In the anionic polyurethane resin (G5), the solids content of the anionic polyurethane resin (G5) was 25% by mass. S The glass transition temperature (Tg) of the resulting anionic polyurethane resin (G5) was measured using a dynamic viscoelasticity measuring device and was found to be 120°C.

[0122] Production method for anionic polyurethane resin (G6) A water-dispersible anionic polyurethane resin (G6) having a solids content of 25% by mass was obtained in the same manner as in the production method for anionic polyurethane resin (G1), except that 100 parts by mass of a polyester polyol having a number average molecular weight of 1,000 obtained from 1,6-hexanediol and adipic acid was used in place of 100 parts by mass of a polyether polyol having a number average molecular weight of 5,000 obtained from polyethylene glycol and polypropylene glycol. S The glass transition temperature (Tg) of the resulting anionic polyurethane resin (G6) was measured using a dynamic viscoelasticity measuring device and was found to be 140°C.

[0123]

[0043] A water-dispersible anionic polyurethane resin (G7) having a solids content of 25% by mass was obtained in the same manner as in the production method for anionic polyurethane resin (G1), except that 100 parts by mass of a polyether polyol having a number average molecular weight of 5,900 obtained from polyethylene glycol and polypropylene glycol was used in place of 100 parts by mass of a polyether polyol having a number average molecular weight of 5,000 obtained from polyethylene glycol and polypropylene.

[0044] In the anionic polyurethane resin (G7), a water-dispersible anionic polyurethane resin (G7) having a solids content of 25% by mass (G S The glass transition temperature (Tg) of the resulting anionic polyurethane resin (G7) was measured using a dynamic viscoelasticity measuring device and was found to be 40°C.

[0124] Production method for anionic polyurethane resin (G8) A water-dispersible anionic polyurethane resin (G8) having a solids content of 25% by mass was obtained in the same manner as in the production method for anionic polyurethane resin (G1), except that 100 parts by mass of a polycarbonate polyol having a number average molecular weight of 6,600 obtained from 1,6-hexanediol and phosgene was used in place of 100 parts by mass of a polyether polyol having a number average molecular weight of 5,000 obtained from polyethylene glycol and polypropylene glycol in the reactor. In the anionic polyurethane resin (G8), the solids content of the anionic polyurethane resin (G8) was 25% by mass. S The glass transition temperature (Tg) of the resulting anionic polyurethane resin (G8) was measured using a dynamic viscoelasticity measuring device and was found to be 20°C.

[0125] Production method for anionic polyurethane resin (G9) A water-dispersible anionic polyurethane resin (G9) having a solids content of 25% by mass was obtained in the same manner as in the production method for anionic polyurethane resin (G1), except that 100 parts by mass of a polycarbonate polyol having a number average molecular weight of 5,300 obtained from 1,6-hexanediol and phosgene was used in place of 100 parts by mass of a polyether polyol having a number average molecular weight of 5,000 obtained from polyethylene glycol and polypropylene glycol in the reactor. In the anionic polyurethane resin (G9), the solids content of the anionic polyurethane resin (G9) was 25% by mass. S The glass transition temperature (Tg) of the resulting anionic polyurethane resin (G9) was measured using a dynamic viscoelasticity measuring device and was found to be 60°C.

[0126] <Silicone Resin (H)> H1: Silicone resin emulsion (solid content: 37% by mass, KM-9782 (registered trademark) manufactured by Shin-Etsu Chemical Co., Ltd.) H2: Silicone resin emulsion (solid content: 15% by mass, WACKER HC321 (registered trademark) manufactured by Wacker Asahi Kasei Silicones Co., Ltd.)

[0127] <Crosslinking agent (I)> I1: Epoxy resin (solid content: 100% by mass, manufactured by Nagase ChemteX Corporation, Denacol (registered trademark) EX-313) I2: Carbodiimide resin (solid content: 40% by mass, manufactured by Nisshinbo Chemical Inc., Carbodilite (registered trademark) SV-02) I3: Oxazoline group-containing polymer (solid content: 40% by mass, manufactured by Nippon Shokubai Co., Ltd., Epocross (registered trademark) K-2020)

[0128] <Phosphate Compound (J)> J1: Diphosphonic acid (C 2 H 8 P 2 O 7 ) J2: Ammonium dihydrogen phosphate (NH 4 (H 2 P.O. 4 )) J3: Phosphoric acid (H 3 P.O. 4 )

[0129] <Fluorine Compound (K)> K1: Ammonium fluoride K2: Potassium fluoride

[0130] <Wax (L)> L1: Polyethylene wax (solid content: 40.0% by mass, manufactured by Mitsui Chemicals, Inc., Chemipearl (registered trademark) W900) L2: Microcrystalline wax (solid content: 46.0% by mass, manufactured by San Nopco Ltd., Nopco (registered trademark) 1245-M-SN)

[0131]

[0132]

[0133]

[0134] (4) Treatment Method: Each of the steel sheets shown in Table 1 (the steel sheet numbers are shown in the "Plated Steel Sheet" column in Table 5) was pretreated, and various test sheets were coated with various first surface treatment solutions (X) shown in Table 2 or Table 4 using a bar coater. Thereafter, without rinsing with water, the test sheets were placed in an oven and dried at the maximum temperature shown in the "PMT" column in Table 5, thereby forming first coatings on both sides with the coating weights (per side) shown in Table 5. Next, various second surface treatment solutions (Y) shown in Table 3 were applied to the surface of the first coating using a bar coater, and then, without rinsing with water, the test sheets were placed in an oven and dried at the maximum temperature shown in the "PMT" column in Table 5, thereby forming second coatings on both sides with the coating weights (per side) shown in Table 5. The coating weights of the first and second coatings were determined by measuring the two-layer coating consisting of the first and second coatings using an X-ray fluorescence analyzer. First, the Zr contained in the two-layer coating was quantified using an X-ray fluorescence analyzer to determine the Zr adhesion amount. Since the Zr contained in the two-layer coating was Zr from the zirconium carbonate compound (C) contained in the first coating, the Zr adhesion amount of the first coating was calculated by converting it from the Zr adhesion amount of the two-layer coating. Next, the Si contained in the two-layer coating was quantified using an X-ray fluorescence analyzer to determine the Si adhesion amount of the two-layer coating. Furthermore, the Si adhesion amount due to the Si of the glycidyl group-containing silane coupling agent (A) and tetraalkoxysilane (B) contained in the first coating was calculated from the adhesion amount of the first coating. The Si adhesion amount of the second coating was calculated by subtracting the Si adhesion amount of the first coating from the Si adhesion amount of the two-layer coating. The Si adhesion amount of the second coating was calculated by converting the Si adhesion amount of the second coating from the Si adhesion amount of the sodium silicate (D2) and silicone resin (H) contained in the second coating.

[0135] (5) Evaluation test methods Samples taken from the obtained zinc-based plated steel sheets with surface treatment films were evaluated in the following items (5-1) to (5-11), and the first surface treatment solution (X) and the second surface treatment solution (Y) were evaluated in the following item (5-12), and the results are shown in Table 5. The evaluation criteria △ and × indicate insufficient performance and are therefore undesirable.

[0136] (5-1) Heat discoloration resistance Each sample was heated to a sheet temperature of 500°C in 30 seconds in an infrared image furnace, held for 5 minutes, and then allowed to cool naturally to room temperature, after which the surface appearance was visually observed. The evaluation criteria are as follows: (Evaluation criteria) ◎: No discoloration ○: Very slight brownish ○-: Slight brownish △: Discolored to brown ×: Discolored to reddish-brown

[0137] (5-2) Heat Cracking Resistance Each sample was heated in an infrared imaging furnace for 30 seconds to a sheet temperature of 500°C, held for 5 minutes, and then allowed to cool naturally to room temperature, after which the surface appearance was visually observed. If no cracks were visible, they were observed at 1000x magnification using an optical microscope. The evaluation criteria are as follows: (Evaluation criteria) ◎: No cracks ○: Very slight cracks ○-: Slight cracks △: Narrow cracks over the entire surface ×: Wide cracks in addition to narrow cracks over the entire surface

[0138] (5-3) Corrosion Resistance of Flat Plates A salt spray test (SST) conforming to JIS-Z-2371-2000 was carried out on each sample in the flat plate state. The corrosion resistance of the flat plate was evaluated based on the area ratio of white rust after 240 hours. The evaluation criteria are as follows: (Evaluation criteria) ◎: White rust area ratio less than 5% ○: White rust area ratio 5% to less than 10% ○-: White rust area ratio 10% to less than 25% △: White rust area ratio 25% to less than 50% ×: White rust area ratio 50% to 100%

[0139] (5-4) Corrosion resistance of bent portion A salt spray test (SST) in accordance with JIS-Z-2371-2000 was carried out on each sample while it was bent at 90° with a 3R. The corrosion resistance of the bent portion was evaluated based on the area ratio of white rust occurring on the top of the head after 144 hours. The evaluation criteria are as follows: (Evaluation criteria) ◎: White rust area ratio of bent portion less than 5% ○: White rust area ratio of bent portion 5% to less than 10% ○-: White rust area ratio of bent portion 10% to less than 25% △: White rust area ratio of bent portion 25% to less than 50% ×: White rust area ratio of bent portion 50% to 100%

[0140] (5-5) Corrosion resistance after alkaline degreasing Alkaline degreasing agent FC-E6406 (manufactured by Nippon Parkerizing Co., Ltd.) was dissolved in pure water at a concentration of 20 g / L and heated to 60°C. Each sample was immersed in this alkaline solution for 2 minutes, removed, washed with water, and dried. A salt spray test (JIS-Z-2371-2000) was conducted on each sample, and the white rust occurrence area rate after 120 hours was evaluated. The evaluation criteria were as shown in (5-3) Evaluation of corrosion resistance of flat plate part above.

[0141] (5-6) Resistance to Blackening Each sample was left for 24 hours in a thermo-hygrostat controlled at an atmosphere of 80°C and 98% relative humidity, and the change in lightness (L value) (ΔL = L value after test - L value before test) was calculated. The evaluation criteria were as follows. The L value was measured in SCI mode (specular reflected light included) using an SR2000 manufactured by Nippon Denshoku Industries Co., Ltd. (Evaluation criteria) ◎: -6<ΔL, and uniform appearance without unevenness ○: -10<ΔL≦-6, and uniform appearance without unevenness ○-: -14<ΔL≦-10, and uniform appearance without unevenness △: -14<ΔL≦-10, and fine black spots present ×: ΔL≦-14, or uneven appearance

[0142] (5-7) Water Stain Resistance For each sample, 100 μL of deionized water was dropped onto the surface of the flat plate, and the sample was placed in a hot air oven with an internal temperature of 100°C for 10 minutes. After removing from the oven, the traces of the water droplets were visually observed to evaluate water stain resistance. The evaluation criteria are as follows: (Evaluation criteria) ◎: The water droplet boundary is not visible regardless of the viewing angle. ○: The water droplet boundary is slightly visible depending on the viewing angle. ○-: The water droplet boundary is slightly visible regardless of the viewing angle. △: The water droplet boundary is clearly visible regardless of the viewing angle. ×: The water droplet boundary is clearly visible beyond the dropping range.

[0143] (5-8) Solvent Resistance A gauze soaked in ethanol was pressed against the surface of each sample under a load of 4.90 N (500 gf), and the surface was rubbed back and forth 10 times while maintaining that load. The rubbed marks were visually evaluated. The evaluation criteria are as follows: (Evaluation criteria) ◎: No traces ○: No traces visible when viewed from above, but clearly visible when viewed from an angle ○-: Traces slightly visible when viewed from above △: Traces clearly visible when viewed from above ×: The coating has peeled off.

[0144] (5-9) Long-term sweat resistance 10 μL of artificial sweat according to JIS-B7001-1995 was dropped onto the surface of each sample, and a silicone rubber stopper was pressed onto the drop to create a site contaminated with artificial sweat of a certain area. This test piece was left to stand for 8 days in a thermo-hygrostat controlled at an atmosphere of 40°C and 80% relative humidity, and then the appearance change of the contaminated site was evaluated. The evaluation criteria are as follows. (Evaluation criteria) ◎: No discoloration ○: Very slight discoloration ○-: Slight discoloration △: Slight blackening ×: Clear blackening

[0145] (5-10) Coating Adhesion Each sample was coated with Delicon (registered trademark) #700 (manufactured by Dai Nippon Toryo Co., Ltd.), a melamine alkyd paint, and baked at 130°C for 30 minutes to form a coating film with a thickness of 30 μm. The sample was then immersed in boiling water for 2 hours, and immediately cut into the steel substrate in a grid pattern (10 x 10 cuts, 1 mm apart). The sample was then extruded 5 mm using an Erichsen extruder so that the cuts faced outward (surface), and the sample was adhered and peeled with adhesive tape, and the peeled area of ​​the coating was measured. The evaluation criteria were as follows. The Erichsen extrusion conditions were in accordance with JIS Z-2247-2006, with a punch diameter of 20 mm, a die diameter of 27 mm, and a drawing width of 27 mm. (Evaluation criteria) ◎: No peeling ○: Peeled area less than 3% ○-: Peeled area 3% or more but less than 10% △: Peeled area 10% or more but less than 30% ×: Peeled area 30% or more

[0146] (5-11) Lubricity A disk-shaped test piece with a diameter of 100 mm was cut out from each sample and molded into a cup shape under the conditions of a punch diameter of 50 mm, a die diameter of 51.91 mm, and a blank holding force of 1 ton. The appearance of the drawn surface of the molded product (the outer side of the cup) was visually inspected, and the degree of scratches and blackening was evaluated. The evaluation criteria are as follows: (Evaluation criteria) ◎: Almost no change over the entire surface, uniform appearance ○: Slight scratches and blackening occurred, and the appearance was clearly uneven ○-: Local scratches and blackening occurred, and the appearance was clearly uneven △: Severe scratches and blackening occurred, mainly in the corners ×: Unable to be molded and cracked

[0147] (5-12) Storage stability Each surface treatment liquid shown in Table 2 was stored in a thermostatic chamber at 40°C for 30 days. After removal, the appearance of each surface treatment liquid was visually inspected and evaluated. The evaluation criteria are as follows: (Evaluation criteria) ◎: No change ○: A very small amount of precipitation was observed ○-: A small amount of precipitation was observed △: A small amount of precipitation was observed and the viscosity increased slightly ×: A large amount of precipitation was observed or the liquid became gelled

[0148]

[0149] As shown in Table 5, the examples of the present invention are excellent in all of the following: heat discoloration resistance, heat cracking resistance, flat part corrosion resistance, processed part corrosion resistance, corrosion resistance after alkaline degreasing, blackening resistance, water stain resistance, solvent resistance, long-term sweat resistance, paint adhesion, and storage stability. Furthermore, the examples of the present invention containing wax were particularly excellent in lubricity. In contrast, the comparative examples, in which any of the requirements fell outside the appropriate range of the present invention, were unable to fully obtain any of the above properties.

[0150] According to the present invention, it is possible to produce a zinc-based plated steel sheet with a surface treatment film that is excellent in all of heat discoloration resistance, heat cracking resistance, corrosion resistance in flat portions, corrosion resistance in processed portions, corrosion resistance after alkaline degreasing, blackening resistance, water stain resistance, solvent resistance, long-term sweat resistance, and paint adhesion.

Claims

1. A surface treatment liquid for zinc-based plated steel sheets, comprising a first surface treatment liquid (X) and a second surface treatment liquid (Y), the first surface treatment liquid (X) containing a silane coupling agent (A) having a glycidyl group, a tetraalkoxysilane (B), a zirconium carbonate compound (C), sodium silicate (D1), a vanadium compound (E), a molybdic acid compound (F), and water, the contents of each component satisfying the following (1) to (6), and the second surface treatment liquid (Y) containing sodium silicate (D2), an anionic polyurethane resin (G), and water, the contents of each component satisfying the following (7) and (8). (1) The solid content mass (A) of the silane coupling agent (A) having a glycidyl group is 100% by mass. S ) the solid content mass (A) of the silane coupling agent (A) having a glycidyl group S ), the solid content mass of tetraalkoxysilane (B) (B S ), and ZrO in the zirconium carbonate compound (C) 2 Converted mass (C Z ) total mass (X S ) to the mass ratio (A S / X S (2) The solid content mass (B) of tetraalkoxysilane (B) is 0.050 to 0.450 S ) the total mass (X S ) to the mass ratio (B S / X S ) is 0.010 to 0.190 (3) ZrO in the zirconium carbonate compound (C) 2 Converted mass (C Z ) the total mass (X S ) to the mass ratio (C Z / X S (4) Solid content mass of sodium silicate (D1) (D1 S ) the total mass (X S ) to mass ratio (D1 S / X S ) is 0.040 to 0.630 (5) The V converted mass (E) of the vanadium compound (E) V ) the total mass (X S ) and the solid content mass of sodium silicate (D1) (D1 S ) and the total mass (X S +D1 S ) to the mass ratio (E V / (X S +D1 S (6) The molybdenum-based mass (F) of the molybdenum acid compound (F) is 0.006 to 0.

094. M ) the total mass (X S ) and the solid content mass of sodium silicate (D1) (D1 S ) and the total mass (X S +D1 S ) to the mass ratio (F M / (X S +D1 S (7) The solid content mass (D2) of sodium silicate (D2) is 0.030 to 0.280 S ) the solid content mass of the anionic polyurethane resin (G) (G S ) to mass ratio (D2 S / G S (8) The solid content mass (G) of the anionic polyurethane resin (G) is 0.010 to 0.100 S ) of the solid content mass (Y) of the second surface treatment liquid (Y S ) to mass ratio (G S / Y S ) is between 0.900 and 0.980 2. The surface treatment solution for zinc-based plated steel sheets according to claim 1, wherein in the second surface treatment solution (Y), the anionic polyurethane resin (G) contains an anionic polyurethane resin having a carbonate skeleton, and the content thereof satisfies the following (9): (9) The ratio of the solid content mass of the anionic polyurethane resin having a carbonate skeleton to the solid content mass of the anionic polyurethane resin (G) (G S ) mass ratio is 0.20 to 0.80 3. The surface treatment solution for zinc-based plated steel sheets according to claim 1 or 2, wherein the second surface treatment solution (Y) further contains a silicone resin (H), the content of which satisfies the following (10). (10) The solid content mass (H) of the silicone resin (H) S ) the solid content mass of the anionic polyurethane resin (G) (G S ) to the mass ratio (H S / G S ) is 0.0030 to 0.0400 4. The second surface treatment solution (Y) for zinc-based plated steel sheets according to any one of claims 1 to 3, further comprising a crosslinking agent (I) whose content satisfies the following (11). (11) The solid content by mass of the crosslinking agent (I) S ) the solid content mass of the anionic polyurethane resin (G) (G S ) to the mass ratio (I S / G S ) is 0.0030 to 0.0400 5. The second surface treatment solution (Y) for zinc-based plated steel sheets according to any one of claims 1 to 4, further comprising wax (L) whose content satisfies the following (12). (12) The solid content (L) of the wax (L) by mass is: S ) of the solid content mass (Y) of the second surface treatment liquid (Y S ) to mass ratio (L S / Y S ) is 0.010 to 0.120 6. The surface treatment solution for zinc-based plated steel sheets according to any one of claims 1 to 5, wherein the first surface treatment solution (X) further contains a phosphoric acid compound (J), the content of which satisfies the following (13). (13) The solid content by mass of the phosphoric acid compound (J) S ) the total mass (X S ) to mass ratio (J S / X S ) is 0.140 to 0.770 7. The surface treatment solution for zinc-based plated steel sheets according to any one of claims 1 to 6, wherein the first surface treatment solution (X) further contains a fluorine compound (K) and the content thereof satisfies the following (14). (14) The solid content mass (K) of the fluorine compound (K) S ) the total mass (X S ) to mass ratio (K S / X S ) is 0.040 to 0.610 8. A method for producing a zinc-based plated steel sheet with a surface treatment film using the surface treatment liquid for zinc-based plated steel sheet according to any one of claims 1 to 7, comprising the steps of: applying the first surface treatment liquid (X) to a surface of a zinc-based plated steel sheet; then drying the applied first surface treatment liquid (X) to form a first film; then applying the second surface treatment liquid (Y) to the surface of the first film; and then drying the applied second surface treatment liquid (Y) to form a second film.

9. The coating weight of the first coating is 0.010 to 0.400 g / m 2 and the coating weight of the second coating is 0.20 to 3.00 g / m 2 The method for producing a zinc-based plated steel sheet having a surface treatment film according to claim 8, 10. A zinc-based plated steel sheet with a surface treatment film, produced by the method for producing a zinc-based plated steel sheet with a surface treatment film according to claim 8 or 9.

11. The zinc-based plated steel sheet with a surface treatment film according to claim 10, wherein the zinc-based plated steel sheet is a hot-dip Zn-Al-based alloy plated steel sheet having, on at least one surface of a base steel sheet serving as a substrate, a hot-dip Zn-Al-based alloy plating layer having a component composition containing, in mass %, 3.0-12.0% Al, 0.2-6.0% Mg, 0.0-0.1% Ni, with the balance being Zn and unavoidable impurities.