Electrolysis system

MYPI2026001559A0Undetermined Publication Date: 2025-03-25ASAHI KASEI KOGYO KABUSHIKI KAISHA +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2026001559
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-09-25
Filing Date
2024-06-28
Publication Date
2025-03-25

AI Technical Summary

Technical Problem

Existing electrolytic systems face inefficiencies in the electrolytic hydrogenation reaction due to excessive water transfer from the anode to the cathode, leading to increased resistance in the electrolyte membrane and decreased current efficiency.

Method used

The system supplies water to the anode as water vapor, controlling humidity to remove ionic impurities and suppress excess water in the electrolyte membrane, allowing water to diffuse back from the cathode to the anode, thereby reducing water transfer with protons to the cathode.

Benefits of technology

This approach improves the current efficiency of the electrolytic hydrogenation reaction by minimizing water transfer with protons, reducing hydrogen generation, and maintaining optimal electrolyte membrane resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2026001559_DRAWING_001
    Figure PI2026001559_DRAWING_001
  • Figure PI2026001559_DRAWING_002
    Figure PI2026001559_DRAWING_002
  • Figure PI2026001559_DRAWING_003
    Figure PI2026001559_DRAWING_003
Patent Text Reader

Abstract

Provided is an electrolysis system in which current efficiency of an electrolytic hydrogenation reaction is improved by restricting the amount of water migrating to a cathode while also supplying moisture to an electrolyte membrane and reducing resistance of the electrolyte membrane. Provided is an electrolysis system including an electrolyte membrane having proton conductivity, a cathode containing a catalyst for an electrochemical reaction involving protons, an anode containing a catalyst for oxidizing water to produce protons, and a structure that supplies water vapor to the anode, wherein the anode catalyst layer contains, in part thereof, an ionomer having proton conductivity, and a ratio of (002) diffraction peak intensity of carbon relative to (110) diffraction intensity of Ir oxide of the anode catalyst layer and ohmic resistance of the electrolysis system are within specific ranges. Fig. 1
Need to check novelty before this filing date? Find Prior Art

Description

Electrolysis System

[0001] The present invention relates to an electrolysis system that can be used to produce a hydride by electrochemically decomposing water to generate oxygen and protons and then hydrogenating a substance to be hydrided through an electrochemical reaction utilizing the generated protons.

[0002] In recent years, there has been a desire for the widespread use of renewable energy sources such as solar, wind, hydroelectric, and geothermal power generation, which are new forms of energy that can reduce carbon dioxide emissions during the generation process compared to energy obtained from thermal power generation. However, renewable energy requires mitigation of output fluctuations, particularly those over medium to long periods. Furthermore, large-scale transportation of renewable energy is relatively difficult. To address this issue, it is effective to convert the electricity obtained from renewable energy into chemical energy. An example of a process for directly converting electricity into chemical energy is the electrochemical system. Secondary batteries, or so-called storage batteries, are an example of an electrochemical system, and are widely used devices that convert and store electricity into chemical energy.

[0003] A promising electrochemical system based on renewable energy would involve installing large-scale solar power generation systems or wind power generation systems in suitable locations around the world, using the renewable energy obtained to produce hydrogen by water electrolysis, converting the hydrogen into a hydrogen energy carrier suitable for transportation, transporting it within the country, and consuming the energy domestically.

[0004] Organic hydrides (organic chemical hydrides) have attracted attention as one type of energy carrier. Examples of organic hydrides include cyclic organic compounds such as cyclohexane, methylcyclohexane, and decalin. Organic hydrides are generally liquid at room temperature and pressure, making them easy to handle. Furthermore, organic hydrides can be electrochemically hydrogenated and chemically dehydrogenated. Therefore, when organic hydrides are used as energy carriers, they can be transported and stored more easily than liquid hydrogen. In particular, when a liquid with properties similar to petroleum is selected as the organic hydride, it has the advantage of being highly compatible with relatively large-scale energy supply systems and can be easily delivered to the end of the energy supply system.

[0005] Conventionally, a known method for producing organic hydrides involves producing hydrogen by water electrolysis using renewable energy, and then adding hydrogen to a substance to be hydrogenated (a dehydrogenated organic hydride) in a hydrogenation reactor to produce an organic hydride.

[0006] In contrast, electrolytic synthesis allows hydrogen to be added directly to the material to be hydrided, thereby simplifying the organic hydride production process. Furthermore, efficiency loss is minimal regardless of the scale, and the organic hydride production apparatus exhibits excellent responsiveness to start-up and shutdown cycles. Regarding such organic hydride production technology, for example, Patent Document 1 discloses an organic hydride production apparatus equipped with an anode that generates protons from water and a cathode that hydrogenates an organic compound having an unsaturated bond. In these organic hydride production apparatuses, water or sulfuric acid is supplied to the anode, which generates oxygen gas at the anode, causing the electrode to become covered with generated bubbles, increasing resistance. However, it is disclosed that the use of a porous electrode, such as a mesh or foam electrode, is preferable to promote the supply of liquid water or sulfuric acid to the anode while avoiding such bubble coverage. Patent Documents 2, 3, and 4 disclose electrochemical reduction apparatuses using a moisture supply means that supplies water or humidified gas to the anode.

[0007] JP 2018-197364 A International Publication No. 2015 / 029366 JP 2003-045449 A JP 2012-72477 A

[0008] In this technology, as disclosed in, for example, Patent Document 1, liquid pure water or sulfuric acid is typically supplied to the anode chamber, but problems include deterioration of the electrolyte membrane due to ion exchange with impurity cations; water accompanying protons moving from the anode to the cathode during electrolysis covers the surface of the catalyst component in the cathode, preventing access of water-insoluble substances to be hydrogenated, such as toluene, to the catalyst component, thereby inhibiting the desired hydrogenation reaction at the cathode, reducing the efficiency of producing target hydrides, such as organic hydrides, and causing excess hydrogen to be generated as a side reaction; and the presence of impurity cations replaces protons in the electrolyte membrane with cations, leading to an increase in the resistance of the electrolyte membrane and a decrease in power efficiency. In particular, in an environment where electrolysis progresses and toluene hydrogenation progresses (i.e., a low toluene content), the frequency of toluene coming into contact with the catalyst decreases, reducing reaction efficiency and resulting in a significant decrease in performance. Furthermore, in studying the present invention, the inventors discovered that while supplying steam to the anode can significantly reduce the amount of migrating water that moves from the anode to the cathode during electrolysis, it also causes a shortage of water in the electrolyte membrane, significantly increasing the resistance of the electrolyte membrane, which in turn increases energy consumption and makes it impossible to continue electrolysis under certain conditions.

[0009] Patent Document 2 discloses a moisture supply means for supplying water or humidified gas to the anode, but the anode is configured to have a catalyst component on the porous substrate, and does not mention any problems or solutions that arise when supplying water as a gas.

[0010] Patent Document 3 discloses a means for supplying water or water vapor to the anode, but does not mention the problem or solution disclosed in the present application of controlling the amount of produced water to suppress the generation of hydrogen as a side reaction.

[0011] Patent Document 4 discloses a means for supplying water or water vapor to the anode, but does not mention the problems and solutions of controlling the water vapor supplied to the anode and the increase in resistance due to condensation, which are disclosed in the present application.

[0012] The present invention has been made in view of the above circumstances, and has an object to provide an electrolysis system that suppresses the amount of water that migrates to the cathode in association with protons that migrate from the anode to the cathode during electrolysis, while simultaneously supplying the necessary water to the electrolyte membrane to reduce the resistance of the electrolyte membrane, thereby improving the current efficiency of the electrolytic hydrogenation reaction.

[0013] The present inventors have therefore discovered that by supplying water as water vapor to the anode while controlling the humidity, ionic impurities can be removed from the water and excess water present in the electrolyte membrane can be suppressed, causing water to move from the cathode to the anode by diffusion, thereby suppressing the amount of water that accompanies protons and moves to the cathode, thereby improving the current efficiency of the electrolytic hydrogenation reaction, and have completed the present invention.

[0014] That is, the present invention is as follows: [1] An electrolysis system comprising: a proton-conductive electrolyte membrane; a cathode provided on one side of the electrolyte membrane and comprising a cathode catalyst layer containing a cathode catalyst for a proton-related electrochemical reaction; an anode provided on the opposite side of the electrolyte membrane and comprising an anode catalyst layer containing an anode catalyst for oxidizing water to produce protons; and a structure for supplying water vapor to the anode, wherein a proton-conductive ionomer is contained in a portion of the anode catalyst layer, and the ratio of the carbon (002) diffraction intensity to the Ir oxide (110) diffraction intensity by X-ray analysis of the anode catalyst layer is 0.10 or less, and the ratio is 0.6 A / cm 2 The ohmic resistance measured at 2 [2] 0.6 A / cm 2 The amount of water transferred from the anode to the cathode, measured by 2 min), more than 10.0 mg / (cm 2[3] The electrolysis system according to [1], wherein the current is 0.6 A / cm 2 or less. 2 The amount of water transferred from the anode to the cathode, measured by 2 min), more than 5.0 mg / (cm 2 The electrolysis system according to claim [1] or [2], wherein the water vapor supply time is 100 s (minutes) or less. [4] The electrolysis system according to any of [1] to [3], wherein the structure for supplying water vapor to the anode further comprises a mechanism for preventing condensation of the vapor. [5] The electrolysis system according to any of [1] to [4], wherein the anode catalyst layer forms a porous layer. [6] The electrolysis system according to any of [1] to [5], wherein the water vapor supplied to the anode is water vapor in a gas inert to electrochemical reaction. [7] The electrolysis system according to any of [1] to [5], wherein the water vapor supplied to the anode is water vapor in air. [8] The electrolysis system according to any of [1] to [6], wherein the relative humidity at the anode of the water vapor supplied by the structure for supplying water as water vapor can be controlled to any value between 70 and 100%. [9] The electrolysis system according to [7], wherein the relative humidity at the anode of the water vapor supplied by the structure for supplying water as water vapor can be controlled to any value between 70 and 100%.

[10] The electrolysis system according to any one of [1] to [9], further comprising a structure for supplying an aromatic compound to the cathode as a reaction substrate for obtaining a target product by a hydrogenation reaction.

[11] The electrolysis system according to

[10] , wherein the aromatic compound is toluene.

[12] The electrolysis system according to

[12] , wherein the electrolyte membrane and the anode catalyst layer form a membrane electrode assembly, and the mass of the anode catalyst in the anode catalyst layer is 0.1 mg / cm per electrode area. 2 5.0mg / cm or more 2

[13] The electrolysis system according to any one of [1] to

[11] , wherein the electrolyte membrane and the cathode catalyst layer form a membrane electrode assembly, and the mass of the cathode catalyst in the cathode catalyst layer is 0.1 mg / cm per electrode area. 2 5.0mg / cm or more 2

[14] A method for operating the electrolysis system according to any one of [1] to

[13] , wherein the relative humidity of water vapor in the anode is controlled to an arbitrary value of 70% or more and 100% or less.

[0015] According to the present invention, by supplying water as water vapor to the anode while controlling the humidity, ionic impurities are removed from the water, and by suppressing the amount of excess water present in the electrolyte membrane, water moves from the cathode toward the anode by diffusion, thereby suppressing the amount of water that accompanies protons and moves to the cathode, improving the current efficiency of the electrolytic hydrogenation reaction and suppressing hydrogen generation, thereby increasing the current efficiency of the desired reaction.

[0016] According to the present invention, an electrolysis system is provided in which the current efficiency of the electrolytic hydrogenation reaction is improved by suppressing the amount of water that migrates to the cathode in association with protons that migrate from the anode to the cathode during electrolysis, and at the same time, supplying the necessary water to the electrolyte membrane to reduce the resistance of the electrolyte membrane.

[0017] 1 is a schematic diagram showing an example of an electrolysis system basic unit constituting the electrolysis system of the present invention; 2 is a graph showing the relationship between current efficiency (ε) and current density (i) in Examples and Comparative Examples; 3 is a graph showing the relationship between voltage and current density (i) in Examples and Comparative Examples; 4 is a graph showing the relationship between the amount of transition water discharged from a hydride outlet and current density (i) in Examples and Comparative Examples; and 5 is a graph showing the relationship between the amount of transition water discharged from a hydride outlet and ohmic resistance in Examples and Comparative Examples.

[0018] The present invention will be described below with reference to the drawings based on preferred embodiments. The embodiments are illustrative and do not limit the invention, and all features and combinations thereof described in the embodiments are not necessarily essential to the invention. Identical or equivalent components, parts, and processes shown in each drawing are designated by the same reference numerals, and redundant descriptions will be omitted where appropriate. Furthermore, the scale and shape of each part shown in each drawing are set for convenience to facilitate explanation and should not be interpreted as limiting unless otherwise specified. Furthermore, when terms such as "first" and "second" are used in this specification or claims, unless otherwise specified, they do not represent any order or importance, but are used to distinguish one configuration from another.

[0019] (Electrolysis System) The electrolysis system of the present invention comprises a proton-conductive electrolyte membrane, a cathode provided on one side of the electrolyte membrane and having a cathode catalyst layer containing a cathode catalyst for a proton-related electrochemical reaction, an anode provided on the opposite side of the electrolyte membrane and having an anode catalyst layer containing an anode catalyst for oxidizing water to produce protons, and a structure for supplying water vapor to the anode. In the electrolysis system of the present invention, a proton-conductive ionomer is contained in a portion of the anode catalyst layer. In the electrolysis system of the present invention, the ratio of the carbon (002) diffraction intensity to the Ir oxide (110) diffraction intensity by X-ray analysis of the anode catalyst layer is 0.10 or less.

[0020] FIG. 1 shows an electrolysis system basic unit 100 that constitutes the electrolysis system of the present invention. The electrolysis system of the present invention can be used as an apparatus (e.g., an organic hydride production apparatus, a hydrogen production apparatus) that electrochemically decomposes water to generate oxygen and protons, and then reduces (e.g., hydrogenation, proton reduction) a product to be reduced (e.g., a product to be hydrided, protons) through an electrochemical reaction using the generated protons to produce a reductant (e.g., a hydride, hydrogen). In the electrolysis system of the present invention, water is supplied to the anode as water vapor, so the amount of water present in the electrolyte membrane and anode catalyst layer can be minimized to the minimum required for electrolysis, and water that has migrated to the cathode as produced water returns to the anode side through the electrolyte membrane by diffusion, thereby suppressing the amount of water that migrates to the cathode side. By suppressing the amount of moisture that moves to the cathode side, it is possible to suppress the impediment to access of water-insoluble substances to be hydrided, such as toluene, to the catalyst, which is caused by the cathode catalyst surface being covered with moisture.When used in the production of hydrides (organic hydrides, etc.), this improves the efficiency of producing hydrides (organic hydrides, etc.) through catalytic reactions, and suppresses causes of reduced power efficiency, such as the generation of excess hydrogen as a side reaction and an increase in the resistance of the electrolyte membrane due to the replacement of protons in the electrolyte membrane with cations due to the presence of cations.

[0021] In FIG. 1 , the proton-conductive electrolyte membrane corresponds to a solid polymer electrolyte membrane 11. The following describes the characteristics of a proton-conductive electrolyte membrane using the solid polymer electrolyte membrane 11 as an example. The solid polymer electrolyte membrane 11 is formed of a proton-conductive material. The solid polymer electrolyte membrane 11 selectively conducts protons while suppressing the mixing and diffusion of substances between the cathode 12 and the anode 17. An ionomer is preferably used as the proton-conductive material. As the ionomer, a cation-exchange polymer can be used. For example, a polymer having an acidic group such as a sulfonic acid group or a carboxyl group, or a fluorinated polymer of such a polymer may be used. Specific examples include perfluorosulfonic acid polymers such as Nafion (registered trademark) and Flemion (registered trademark), and (meth)acrylic acid-based fluoropolymers. Among these, perfluorosulfonic acid polymers are most preferred. The thickness of the solid polymer electrolyte membrane 11 is not particularly limited, but is preferably 5 μm or more, more preferably 10 μm or more, even more preferably 20 μm or more, and preferably 300 μm or less, more preferably 200 μm or less, and even more preferably 190 μm or less. By making the thickness of the solid polymer electrolyte membrane 11 5 μm or more, the barrier properties of the solid polymer electrolyte membrane 11 can be ensured and the occurrence of cross-leak of substances to be hydrided, hydrides (organic hydrides), oxygen, etc. can be more reliably suppressed. Furthermore, by making the thickness of the solid polymer electrolyte membrane 11 300 μm or less, excessive ion migration resistance can be suppressed.

[0022] The area resistance of the solid polymer electrolyte membrane 11 immersed in distilled water at 25° C. for 2 hours, i.e., the ion transfer resistance per geometric area, is not particularly limited, but is preferably 2000 mΩ·cm 2 or less, and more preferably 1000 mΩ cm 2 and more preferably 500 mΩ cm or less. 2 The area resistance of the solid polymer electrolyte membrane 11 is set to 2000 mΩ cm or less. 2By setting the ion exchange capacity to 0.7 meq / g or less, the risk of insufficient proton conductivity can be more reliably avoided. When a cation exchange polymer is used as the ionomer, the ion exchange capacity (IEC) is not particularly limited, but is preferably 0.7 to 2 meq / g, and more preferably 1 to 1.3 meq / g. By setting the ion exchange capacity of the cation exchange ionomer to 0.7 meq / g or more, the risk of insufficient ion conductivity can be more reliably avoided. On the other hand, by setting the ion exchange capacity to 2 meq / g or less, the risk of insufficient strength of the solid polymer electrolyte membrane 11 due to increased solubility of the ionomer in the anode fluid, the substance to be hydrogenated, organic hydride, etc. can be more reliably avoided.

[0023] The solid polymer electrolyte membrane 11 may be mixed with a reinforcing material made of a corrosion-resistant polymer such as a fluoropolymer (e.g., PTFE (polytetrafluoroethylene), Viton (trademark) (fluoroelastomer)). By introducing the reinforcing material, it is possible to suppress a decrease in the dimensional stability of the electrolyte membrane 11, thereby improving the durability of the electrolyte membrane 11. It is also possible to suppress crossover of substances to be hydrided, organic hydrides, oxygen, and the like. The surface of the solid polymer electrolyte membrane 11 may be made hydrophilic by coating it with a predetermined inorganic layer (e.g., platinum, ruthenium, palladium, iridium, or an alloy containing one or more of these). By making the membrane hydrophilic, it is possible to improve the desorption of generated oxygen bubbles and thereby improve performance.

[0024] The cathode 12 is provided on one side of the solid polymer electrolyte membrane 11. In this embodiment, the cathode 12 is provided so as to be in contact with one main surface of the electrolyte membrane 11. The space accommodating the cathode 12 may also be referred to as the "cathode chamber." The cathode 12 contains a cathode catalyst for an electrochemical reaction involving protons. The cathode 12 may have a structure in which, for example, a cathode catalyst layer 12a containing the cathode catalyst and a cathode substrate / porous flow path 12b are stacked. In this case, the cathode catalyst layer 12a is preferably provided so as to be in contact with one main surface of the electrolyte membrane 11. The main surface of the cathode substrate / porous flow path 12b opposite the cathode catalyst layer 12a may be in contact with the cathode-side bipolar plate 16a.

[0025] The cathode catalyst layer 12a includes a cathode catalyst (reduction catalyst) for a proton-related electrochemical reaction. Examples of proton-related electrochemical reactions include a reaction in which a substance to be hydrided is hydrogenated with protons to produce a hydride (organic hydride). The cathode catalyst may be, for example, metal particles selected from the group consisting of Pt, Ru, Pd, Ir, and alloys containing at least one of these. The cathode catalyst may be a commercially available product or one prepared according to a known method. The cathode catalyst may also be composed of a metal composition containing a first catalytic metal (noble metal) consisting of at least one of Pt, Ru, Pd, and Ir and one or more second catalytic metals selected from Cr, Mn, Fe, Co, Ni, Cu, Zn, Mo, Ru, Sn, W, Re, Pb, and Bi. In this case, the metal composition may be in the form of an alloy of the first catalytic metal and the second catalytic metal, or an intermetallic compound made of the first catalytic metal and the second catalytic metal.

[0026] The cathode catalyst may be supported by a catalyst support made of an electron-conductive material. Supporting the cathode catalyst on a catalyst support can increase the surface area of ​​the cathode catalyst layer 12a. Furthermore, agglomeration of the cathode catalyst can be suppressed. Porous fine particles can be used as the catalyst support. Examples of the catalyst support include electron-conductive materials containing porous carbon (such as mesoporous carbon), porous metals, or porous metal oxides as the main component, and porous metal compounds such as metal nitrides, carbides, oxynitrides, carbonitrides, and partially oxidized carbonitrides.

[0027] Examples of porous carbon include carbon blacks such as Ketjen Black (registered trademark), acetylene black, furnace black, and Vulcan (registered trademark). Examples of porous metals include Pt black, Pd black, and fractally precipitated Pt metal. Examples of metal elements constituting porous metal oxides or other metal compounds include Ti, Zr, Nb, Mo, Hf, Ta, and W. When using porous metals, the porous metal itself, without supporting metal particles, may be used as the cathode catalyst. The average particle size of the porous microparticles used as the catalyst support or porous metal catalyst is preferably 0.01 μm to 1 μm.

[0028] The catalyst support or porous metal catalyst supporting the cathode catalyst may be coated with an ionomer. This can improve ionic conductivity within the cathode catalyst layer 12a. Examples of the ionomer include those exemplified as examples of ionomers that can be used as materials for the solid polymer electrolyte membrane 11. The ionomer contained in the cathode catalyst layer 12a preferably partially coats the cathode catalyst. This allows the three elements (products to be hydrided, protons, and electrons) necessary for the electrochemical reaction in the cathode catalyst layer 12a to be efficiently supplied to the reaction field.

[0029] The thickness of the cathode catalyst layer 12a is preferably 1 to 100 μm, and more preferably 5 to 30 μm. As the thickness of the cathode catalyst layer 12a increases, not only does the resistance to proton transfer increase, but the diffusibility of the substance to be hydrogenated and the organic hydride also decreases. For this reason, it is desirable to adjust the thickness of the cathode catalyst layer 12a within the above-mentioned range.

[0030] The cathode catalyst layer 12a can be produced, for example, by the following method. First, catalyst component powder, water, a solvent such as 1-propanol, and an ionomer (for example, Nafion (registered trademark) dispersion DE521 (manufactured by DuPont)) are mixed. The amount of ionomer added is preferably such that the ratio of the mass of the ionomer to the mass of carbon in the catalyst component powder after drying is 1:10 to 10:1. Optionally, a suitable solvent is added to the resulting mixture to prepare a catalyst ink.

[0031] Next, the obtained catalyst ink is applied to the cathode substrate / porous flow channel 12b, dried, and then hot-pressed to fix the cathode catalyst layer 12a to the cathode substrate / porous flow channel 12b. It is preferable to perform the above-mentioned application and drying steps multiple times before hot-pressing. This allows for a more homogeneous cathode catalyst layer 12a to be obtained. The cathode catalyst layer 12a can be produced through the above steps. The cathode catalyst layer 12a may also be formed on the solid polymer electrolyte membrane 11. For example, a composite of the cathode catalyst layer 12a and the solid polymer electrolyte membrane 11 can be produced by applying the catalyst ink to one main surface of the solid polymer electrolyte membrane 11 using a bar coater. Alternatively, the cathode catalyst layer 12a and the solid polymer electrolyte membrane 11 can be produced by spraying the catalyst ink onto one main surface of the solid polymer electrolyte membrane 11 and then drying the solvent component in the catalyst ink. Alternatively, the cathode catalyst layer 12a and the solid polymer electrolyte membrane 11 can be produced by spraying the catalyst ink onto a PTFE substrate, and then transferring the ink to the solid polymer electrolyte membrane 11 under heated conditions using a press or the like. In these cases, the solid polymer electrolyte membrane 11 and the cathode catalyst layer 12a can be considered to form a membrane electrode assembly. The catalyst ink is preferably used in such a manner that the mass of the cathode catalyst (reducing catalyst, e.g., catalytic metal) in the cathode catalyst layer 12a is 0.1 mg / cm per electrode area. 2 More preferably, 0.2 mg / cm 2 More preferably, 0.3 mg / cm 2 or more, preferably 5.0 mg / cm 2 or less, more preferably 3.0 mg / cm 2 More preferably, 1.0 mg / cm or less 2 The cathode catalyst may be applied so that the mass of the cathode catalyst in the cathode catalyst layer 12a is equal to or greater than the above-mentioned lower limit, which reduces reaction resistance and contributes to improving electrolysis performance. The mass of the cathode catalyst in the cathode catalyst layer 12a is equal to or less than the above-mentioned upper limit, which reduces the thickness of the catalyst layer and suppresses ion migration resistance.

[0032] The cathode substrate / porous flow channel 12b functions to uniformly distribute the liquid material to be hydrided, supplied from the outside, across the surface of the cathode catalyst layer 12a. The material constituting the cathode substrate / porous flow channel 12b preferably has a high affinity for the material to be hydrided and the hydride (organic hydride). Examples of materials constituting the cathode substrate / porous flow channel 12b include porous conductive substrates and sintered fibers. These are preferred because they have porosity suitable for supplying the liquid material to be hydrided and removing the liquid hydride and by-products, while maintaining sufficient electrical conductivity. The thickness of the cathode substrate / porous flow channel 12b is selected to optimize the pressure loss within the cathode substrate / porous flow channel 12b associated with supplying the liquid material to be hydrided to the cathode catalyst layer 12a and removing the liquid hydride and by-products, and is preferably 10 to 5,000 μm.

[0033] More specific examples of materials constituting the cathode substrate / porous flow path 12b include woven carbon fabric (carbon cloth), nonwoven carbon fabric, and carbon paper. Carbon cloth is made by bundling hundreds of thin carbon fibers with diameters of a few μm together and then woven into a fabric. Carbon paper is made by sintering a thin film precursor made from raw carbon fiber using a papermaking method. The cathode substrate / porous flow path 12b is provided with an inlet 13 for the material to be hydrided and an outlet 14 for the material to be hydrided, which communicate the inside and outside of the cathode substrate / porous flow path 12b.

[0034] The cathode 12 is preferably provided with a material to be hydrided inlet 13 as a means for supplying the material to be hydrided to the cathode 12, and a hydride outlet 14 as a means for recovering the hydride produced at the cathode 12. For example, the material to be hydrided inlet 13 may be arranged below the cathode 12, and the hydride outlet 14 may be arranged above the cathode 12 and vertically above the material to be hydrided inlet 13. One end of the material to be hydrided inlet 13 and the hydride outlet 14 may be connected to the cathode substrate / porous flow channel 12b. Furthermore, the other end of one or both of the material to be hydrided inlet 13 and the hydride outlet 14 may be connected to a catholyte storage tank (not shown) for storing catholyte (a collective term for the material to be hydrided-containing liquid supplied to the cathode 12 and the hydride-containing liquid discharged from the cathode 12). A cathode liquid transport device (not shown) constituted by various pumps such as a gear pump or a cylinder pump, or a gravity flow device, may be provided between the to-be-hydrided product inlet 13 and / or the hydride outlet 14 and the cathode liquid storage tank. When the to-be-hydrided product inlet 13 and the hydride outlet 14 are both connected to the cathode liquid storage tank, the cathode liquid is gradually hydrogenated by an electrochemical reduction reaction at the cathode 12 while circulating within the system.

[0035] The cathode solution storage tank contains a liquid containing a substance to be hydrogenated by an electrochemical reduction reaction in this electrolysis system, a liquid containing a hydrogenated hydride, or a circulating liquid that is gradually hydrogenated. The combination of organic hydride dehydrogenation product (substance to be hydrogenated) and organic hydride (hydride) used in this embodiment is not particularly limited as long as it is a combination of organic compounds that can add / desorb hydrogen by reversible hydrogenation / dehydrogenation reactions. Furthermore, a combination in which the substance to be hydrogenated and the hydride are liquid is preferred. A wide variety of combinations, such as acetone-isopropanol systems, benzoquinone-hydroquinone systems, and aromatic hydrocarbon-aromatic hydrocarbon hydride systems, can be used. The aromatic hydrocarbon compound used as the dehydrogenated organic hydride is a compound containing at least one aromatic ring, such as benzene or alkylbenzene. Alkylbenzenes include compounds in which one to four hydrogen atoms on the aromatic ring are substituted with linear or branched alkyl groups having one to two carbon atoms, such as toluene and xylene. These may be used alone or in combination. The aromatic hydrocarbon compound is preferably at least one of toluene and benzene. Nitrogen-containing heterocyclic aromatic compounds such as pyridine, pyrimidine, and pyrazine can also be used as dehydrogenated products. The organic hydride is a hydrogenated version of the above-mentioned dehydrogenated product, and examples thereof include methylcyclohexane, dimethylcyclohexane, and piperidine.

[0036] The dehydrogenated organic hydride, i.e., the material to be hydrogenated, is preferably a liquid at room temperature. When a mixture of multiple types of the above-mentioned aromatic hydrocarbon compounds and / or nitrogen-containing heterocyclic aromatic compounds is used, the mixture only needs to be liquid. When the material to be hydrogenated is a liquid at room temperature, it can be supplied to the cathode 12 in a liquid state without treatment such as heating or pressurization. This allows for a simplification of the configuration of the electrolysis system.

[0037] Furthermore, when producing hydrogen instead of a liquid hydride, the means from the cathode solution storage tank to the product to be hydrided inlet 13 and the means for the hydride outlet 14 are unnecessary. Among these, when the purpose is to transport energy by ship or vehicle, aromatic hydrocarbon-aromatic hydrocarbon hydride systems, such as toluene-methylcyclohexane systems, are preferred from the viewpoints of transportability, toxicity, safety, storage stability, etc., as well as energy conversion efficiency, such as the amount of hydrogen that can be transported per volume or mass, ease of hydrogenation and dehydrogenation reactions, and a relatively small change in Gibbs free energy. The product to be hydrided may be supplied to the cathode 12 in its original state (i.e., 100%), or may be supplied to the cathode 12 as a solution in which it is dissolved in a solvent (e.g., a common organic solvent such as cyclohexane or methylcyclohexane is used. Organic solvents without double bonds are preferably used because they have weak adsorptivity and are less likely to be reduced). In the case of a solution, the concentration of the product to be hydrided may be, for example, 1 to 100% vol / vol.

[0038] A cathode-side spacer 15 is preferably provided to seal the upper and lower sides of the cathode 12 and to protect the material to be hydrided inlet 13 and the material to be hydrided outlet 14. The cathode-side spacer 15 may be provided, for example, below and above the cathode 12 in close contact with the cathode 12 so as to enclose the material to be hydrided inlet 13 and the material to be hydrided outlet 14. The cathode-side spacer 15 serves as a sealant that prevents the material to be hydrided and the organic material containing the hydride from leaking out of the cathode substrate and porous flow path 12b, and is preferably electronically insulating. Examples of materials that constitute the cathode-side spacer 15 include corrosion-resistant polymers such as fluoropolymers (e.g., PTFE (polytetrafluoroethylene), Viton (trademark) (fluoroelastomer)).

[0039] The cathode bipolar plate 16a may be disposed in contact with the cathode substrate / porous flow path 12b. In this embodiment, the cathode bipolar plate 16a is laminated on the main surface of the cathode substrate / porous flow path 12b opposite the cathode catalyst layer 12a. The cathode bipolar plate 16a has electronic conductivity and also functions as a power supply plate. Examples of materials that can be used for the cathode bipolar plate 16a include metals such as SUS and Ti.

[0040] The anode 17 is provided on the other side of the solid polymer electrolyte membrane 11. In this embodiment, the cathode 12 is provided in contact with one main surface of the solid polymer electrolyte membrane 11, and therefore the anode 17 is provided on the opposite main surface of the solid polymer electrolyte membrane 11. The anode 17 may be composed of, for example, a porous anode catalyst layer 17a, or may have a structure in which the anode catalyst layer 17a and an anode substrate 17b are laminated together. The anode 17 may be provided between the solid polymer electrolyte membrane 11 and the anode flow channel structure 18. When the anode 17 is composed of the anode catalyst layer 17a, one main surface of the anode catalyst layer 17a can be provided in contact with the solid polymer electrolyte membrane 11, and the other main surface of the anode catalyst layer 17a can be provided in contact with the anode flow channel structure 18. In these cases, the solid polymer electrolyte membrane 11 and the anode catalyst layer 17a can be considered to form a membrane electrode assembly. When the anode 17 has a structure in which an anode catalyst layer 17a and an anode substrate 17b are stacked, the anode catalyst layer 17a may be in contact with one main surface of the solid polymer electrolyte membrane 11, and the main surface of the anode substrate 17b opposite the anode catalyst layer 17a may be in contact with the anode flow channel structure 18. An anode-side bipolar plate 16b may be disposed on the main surface of the anode flow channel structure 18 opposite the anode 17, in contact with the anode flow channel structure 18. Examples of materials constituting the anode-side bipolar plate 16b include those exemplified as materials constituting the cathode-side bipolar plate 16a. When the electrolysis system of the present invention has a repeating structure in which electrolysis system basic units 100 as shown in FIG. 1 are repeated as repeating units, the anode-side bipolar plate 16b also serves as the cathode-side bipolar plate 16a of the electrolysis system basic unit adjacent to the anode side, except for the electrolysis system basic units at the end.

[0041] The anode catalyst layer 17a includes an anode catalyst (oxidation catalyst) for oxidizing water to generate protons. The reaction for oxidizing water to generate protons includes the decomposition of water into oxygen and protons. For example, particles of Ir or Ru oxide or a composite oxide containing at least one of these can be used as the anode catalyst. The anode catalyst may be a commercially available product or one prepared according to a known method. The mass of the anode catalyst (oxidation catalyst, e.g., catalytic metal oxide) in the anode catalyst layer 17a per electrode area is preferably 0.1 mg / cm. 2 More preferably, 0.2 mg / cm 2 More preferably, 0.3 mg / cm 2 or more, preferably 5.0 mg / cm 2 or less, more preferably 3.0 mg / cm 2 More preferably, 1.0 mg / cm or less 2 If the mass of the anode catalyst in the anode catalyst layer 17a is equal to or greater than the above-mentioned lower limit, the reaction resistance can be reduced, contributing to improved electrolysis performance. If the mass of the anode catalyst in the anode catalyst layer 17a is equal to or less than the above-mentioned upper limit, the catalyst layer thickness can be reduced, and ion migration resistance can be suppressed.

[0042] The anode catalyst may be supported by a catalyst support. Examples of catalyst supports include carbon and non-carbon materials, with non-carbon materials being preferred. The presence of a carbon material in the anode may result in oxidation, resulting in a decrease in current efficiency. The carbon content in the anode catalyst layer 17a is preferably 30 wt % or less, more preferably 10 wt % or less, even more preferably 1 wt % or less, and most preferably approximately 0 wt %.

[0043] The carbon content in the anode catalyst layer 17a can be qualitatively determined by the ratio of the diffraction intensity of carbon to the diffraction intensity of Ir oxide, measured by wide-angle X-ray diffraction, for example. Specifically, the ratio of the diffraction intensity of carbon (002) diffraction, which appears at a diffraction angle of about 26 degrees, to the diffraction intensity of Ir oxide (110) diffraction, which appears at a diffraction angle of about 28 degrees, measured by CuKα radiation ((002) C / (110) IrO2 When two diffraction peaks overlap and cannot be clearly separated, the ratio of the intensity of the (10) diffraction of carbon, which appears at a diffraction angle of about 42-43 deg, to the intensity of the (200) diffraction of Ir oxide, which appears at a diffraction angle of about 39 deg, can be calculated as ((10) C / (200) IrO2 ) can also be calculated as (002) C / (110) IrO2 and (10) C / (200) IrO2 From the viewpoint of suppressing a decrease in current efficiency, the values ​​of are preferably 0.1 or less and 0.2 or less, respectively.

[0044] The anode catalyst layer 17a includes a proton-conductive ionomer in a portion thereof. In this embodiment, "including an ionomer" means that the ionomer is present in the pores of the porous layer, and may also mean, for example, that the anode catalyst layer 17a is "coated with the ionomer." This improves the ionic conductivity within the anode catalyst layer 17a. Examples of the ionomer include those exemplified as ionomers that can be used as materials for the solid polymer electrolyte membrane 11. The ionomer included in the anode catalyst layer 17a preferably partially coats the anode catalyst. This allows water, which is necessary for the electrochemical reaction in the anode catalyst layer 17a, to be supplied to the reaction field, and protons, electrons, and oxygen to be discharged from the reaction field.

[0045] The type of ionomer present in the anode catalyst layer 17a can be identified by known methods, such as microscopic Fourier transform infrared spectroscopy and solid-state 19F NMR, or analyzed using X-ray photoelectron spectroscopy (XPS).

[0046] The mass fraction of the ionomer present in the anode catalyst layer 17a is 1 wt % or more, preferably 5 wt % or more, and more preferably 10 wt % or more, from the viewpoint of capturing moisture supplied to the anode and improving the proton conductivity of the electrolyte membrane. Furthermore, from the viewpoint of maintaining a good catalytic reaction and reducing ionic resistance, it is preferably 50 wt % or less, more preferably 40 wt % or less, and even more preferably 30 wt % or less. The mass fraction of the ionomer present in the anode catalyst layer can be measured, for example, using a scanning electron microscope with energy dispersive X-ray fluorescence (SEM-EDX) analysis. The scanning electron microscope is a Hitachi High-Technologies SU8010, and the EDX is a Horiba EMAX Evolution, with an acceleration voltage of 10 kV and a magnification of 1 kV. The target elements, C, O, F, S, and Ir, are measured at any location in the anode catalyst layer. If an ionomer is present in the anode catalyst layer, element peaks for all of the target elements are observed. The proportion of the ionomer in the anode catalyst layer measured by EDX can be measured as the ratio of the mass % of the peak of F element to the mass % of the peak of Ir element. From the viewpoint of capturing water and improving the proton conductivity of the electrolyte membrane, the ratio is preferably 0.01 or more, more preferably 0.03 or more, and even more preferably 0.05 or more, and from the viewpoint of maintaining a good catalytic reaction and reducing ionic resistance, the ratio is preferably 1.00 or less, more preferably 0.80 or less, and even more preferably 0.70 or less.

[0047] The thickness of the anode catalyst layer 17a is preferably 1 to 100 μm, and more preferably 5 to 30 μm. As the thickness of the anode catalyst layer 17a increases, not only does the resistance to proton transfer increase, but the diffusibility of water and oxygen also decreases. For this reason, it is desirable to adjust the thickness of the anode catalyst layer 17a within the above-mentioned range.

[0048] The ratio of the carbon (002) diffraction intensity to the Ir oxide (110) diffraction intensity in the anode catalyst layer 17a must be 0.10 or less, preferably 0.05 or less, and more preferably no carbon (002) diffraction peak is detected (i.e., the ratio of the carbon (002) diffraction intensity to the Ir oxide (110) diffraction intensity is approximately 0). The magnitude of the ratio of the carbon (002) diffraction intensity to the Ir oxide (110) diffraction intensity in the anode catalyst layer 17a reflects the carbon content in the anode catalyst layer. For example, if no carbon (002) diffraction peak is detected (i.e., the ratio of the carbon (002) diffraction intensity to the Ir oxide (110) diffraction intensity is approximately 0), this reflects that the carbon content in the anode catalyst layer 17a is approximately 0 wt %. When the ratio of the (002) diffraction intensity of carbon to the (110) diffraction intensity of Ir oxide in the anode catalyst layer 17a is equal to or less than the upper limit, current consumption due to oxidation of carbon can be suppressed.

[0049] The anode catalyst layer 17a may form a porous layer. When the anode catalyst layer 17a forms a porous layer, the anode catalyst layer 17a may contain a proton-conductive ionomer in some of the pores of the porous layer. The porosity and other properties of the porous layer that the anode catalyst layer 17a can form can be analyzed, for example, by the following method.

[0050] The porosity (V) of the anode catalyst layer 17a formed on the PTFE sheet or the anode catalyst layer 17a in the membrane electrode assembly p,CL ) is the bulk density (ρ bulk,CL ) and true density (ρ real,CL ) is calculated using the following formula: p,CL = 1 - ρ bulk,CL / ρ real,CL When measuring the density of the anode catalyst layer 17a formed on the PTFE sheet or the anode catalyst layer 17a in the membrane electrode assembly, the cathode catalyst layer 12a is removed, and the laminate consisting of the PTFE sheet and the anode catalyst layer 17a or the laminate consisting of the solid polymer electrolyte membrane 11 and the anode catalyst layer 17a is subjected to the measurement.

[0051] The bulk density (ρ bulk,CL ) is calculated according to the following procedure. First, the mass of the anode catalyst layer 17a alone is calculated by subtracting the mass of the PTFE sheet or solid polymer electrolyte membrane 11 cut to a predetermined size from the mass of the laminate consisting of the PTFE sheet and the anode catalyst layer 17a, or the mass of the laminate consisting of the solid polymer electrolyte membrane 11 and the anode catalyst layer 17a, of the same size. Next, the thickness of the anode catalyst layer 17a alone is calculated by observing the cross section with a scanning electron microscope. Finally, the bulk density (ρ ) of the anode catalyst layer 17a alone is calculated by dividing the mass of the anode catalyst layer 17a alone by its size and thickness. bulk,CL ) is calculated.

[0052] The true density (ρ real,CL ) can be measured using a density meter (e.g., dry automatic density meter Accupyc II 1345 (Shimadzu Corporation)). First, the mass (M c ) from the mass (M s ) to reduce the mass of the anode catalyst layer 17a alone (M CL Next, the true density (ρ real,c Next, the true density (ρ real,s Finally, the true density (ρ real,CL ) is calculated. real,CL =M CL / (M c / ρ real,c -M s / ρ real,s )

[0053] Whether the anode catalyst layer is porous can also be confirmed by cutting out a cross section of the anode catalyst layer using, for example, a cryomicrotome and observing the voids present in the cross section using a scanning electron microscope.

[0054] The anode substrate 17b functions to uniformly diffuse water from the outside into the anode catalyst layer 17a. The material constituting the anode substrate 17b is stable in the strongly oxidizing environment of the anode catalyst layer 17a and also provides electronic conduction between the anode catalyst layer 17a and the anode flow channel structure 18, so it is preferable that the material have high electronic conductivity. Examples of materials constituting the anode substrate 17b include porous conductive substrates and sintered fiber bodies. These are preferred because they have porosity suitable for supplying and removing gases and liquids and can maintain sufficient electrical conductivity. The thickness of the anode substrate 17b is preferably 10 to 5,000 μm.

[0055] More specific examples of materials constituting the anode substrate 17b include titanium fiber sintered compacts and porous titanium sintered compacts plated with an electronic conductor such as Pt, Ir, or Ru to enhance the electronic conductivity of the surface.

[0056] The electrolysis system of the present invention further includes a structure for supplying water vapor to the anode (hereinafter, abbreviated as "water vapor supply structure"). The water vapor supplied to the anode may be water vapor in an inert gas (i.e., a mixed gas of water vapor and an inert gas). The water vapor supply structure may include, for example, a means for generating a mixed gas of water vapor and an inert gas (corresponding to the humidifier main body 23 in FIG. 1 ), a means for introducing the mixed gas into the anode (corresponding to the humidified gas inlet 20 in FIG. 1 ), a space for storing the mixed gas in the anode (corresponding to the anode chamber 19 in FIG. 1 ), and a means for discharging excess gas (corresponding to the humidified gas outlet 21 in FIG. 1 ). To form an area (anode chamber 19) for storing the mixed gas in the anode, an anode flow channel structure 18 may be provided between the anode 17 and the anode-side bipolar plate 16b (i.e., between the anode catalyst layer 17a and the anode-side bipolar plate 16b when the anode substrate 17b is not present, or between the anode substrate 17b and the bipolar plate 16b when the anode substrate 17b is present). The anode flow channel structure 18 is responsible for electronic conduction between the anode 17 and the anode-side bipolar plate 16b and forms the space of the anode chamber 19 for supplying a gas containing feed water 25 to the anode 17. The anode flow channel structure 18 may be, for example, a cylindrical structure formed with a frame made of a rigid conductive material (e.g., metal). The thickness of the anode flow channel structure 18 is preferably 0.2 to 1.0 mm, more preferably 0.4 to 0.7 mm. The humidified gas inlet 20 may be arranged, for example, so that one end is connected to the bottom of the anode chamber 19 and the other end is connected to the humidifier main body 23. A gas that is not involved in the reaction at the anode catalyst layer 17a is introduced into the humidifier main body 23 through an inert gas inlet 24, and the feed water 25 is supplied as steam to the anode chamber 19 through the humidified gas inlet 20. As the inert gas, not only electrochemically inert gases such as nitrogen and rare gases (e.g., helium, neon, argon, krypton, xenon, etc.) but also air can be used. From the viewpoint of simplicity, air is preferred as the inert gas. Furthermore, the humidified gas outlet 21 may be arranged vertically above the humidified gas inlet 20.

[0057] The water vapor supply structure may have a structure that prevents condensation of the steam. For example, known methods such as covering with a heat-insulating material or heating with a heater can be used. In the electrolysis system of the present invention, electrolysis is performed by supplying the minimum amount of water necessary to the anode catalyst layer and the electrolyte membrane, so controlling the supply of water in a vapor state is important. Preventing condensation of the supplied steam suppresses loss of the water supply amount, and controlling the amount of water supplied to the anode catalyst layer and the electrolyte membrane prevents an increase in resistance due to a lack of water and achieves high current efficiency by suppressing migration of water. Furthermore, preventing condensation contributes to preventing blockage of the flow path in the anode chamber due to condensed water and local swelling of the electrolyte membrane, thereby improving durability during long-term use.

[0058] An anode-side spacer 22 is preferably provided to seal the area below and above the anode 17 and to protect the humidified gas inlet 20 and the humidified gas outlet 21. The anode-side spacer 22 may be provided, for example, below and above the anode 17 in close contact with the anode 17 so as to enclose the humidified gas inlet 20 and the humidified gas outlet 21. The anode-side spacer 22 also serves as a sealant that prevents the mixed gas of water vapor and inert gas from leaking outside the anode chamber 19, and is preferably electronically insulating. Examples of materials that constitute the anode-side spacer 22 include corrosion-resistant polymers such as fluoropolymers (e.g., PTFE (polytetrafluoroethylene)).

[0059] In the electrolysis system of the present invention, the relative humidity of the water vapor supplied by the water vapor supply structure at the location of the anode can be controlled to any value, preferably between 70 and 100%, more preferably between 80 and 100%, and even more preferably between 90 and 100%. The relative humidity of the water vapor can be controlled, for example, by adjusting the heating temperature of the humidifier body 23 or the amount of inert gas mixed therein, and optionally by measuring the humidity at the anode and providing feedback.

[0060] In the electrolysis system of the present invention, the ohmic resistance fluctuates because the amount of water in the electrolyte membrane varies depending on the conditions of the water vapor supplied to the anode. For example, when the amount of water vapor supplied is insufficient, the amount of water in the electrolyte membrane is insufficient, so the amount of water transferred to the cathode can be kept low, but the resistance of the electrolyte membrane increases. When the amount of water vapor supplied is excessive, the electrolyte membrane is sufficiently humidified and the resistance is reduced, but condensation occurs in the anode chamber and in the path for supplying water vapor. It is important to control the resistance and amount of water transferred in the electrolysis system within appropriate ranges.

[0061] The electrolysis system of the present invention has a capacitance of 0.6 A / cm 2 The ohmic resistance measured at is preferably 0.400 Ω cm from the viewpoint of reducing the potential during electrolysis, reducing energy consumption, and reducing hydrogen generation due to side reactions. 2 Below 0.350 Ωcm is good. 2 Preferably, 0.300 Ωcm or less 2 Preferably, 0.280 Ωcm or less 2 The following is preferred:

[0062] The ohmic resistance was measured by stabilizing the operating temperature, the liquid supply rate to the cathode chamber, and the supply rate to the anode chamber, and then measuring 0.6 A / cm 2 The ohmic resistance at 0.60 A / cm can be measured by the method described in the Examples. Specifically, the organic hydride production apparatus is connected to an electrochemical property evaluation apparatus (VSP300, manufactured by Biologic), and after adjusting the organic hydride production apparatus to the operating conditions, 2 After holding at 40°C for 30 seconds, impedance measurement was carried out under the following conditions. From the obtained Nyquist plot, the ohmic resistance (Ω cm) was calculated by multiplying the intersection of the plot on the high frequency side with the real axis by the electrode area. 2 ) was calculated. Current density: 0.60 A / cm 2 Amplitude: 40 mA Frequency: 100.0 kHz to 10.0 mHz Number of measurement points: 6 / decade In the case of a single cell or stacked cells, the operating temperature, the liquid supply rate to the cathode, and the supply rate to the anode chamber can be stabilized before performing the following measurement. 2Apply current and stabilize voltage V 1 , current density 0.7 A / cm 2 The voltage immediately after changing to V 2 The voltage change width at that time is ΔV 12 Again, 0.6 A / cm 2 Apply current at V and stabilize the voltage. 3 , current density 0.6 A / cm 2 The voltage immediately after changing to V 4 The voltage change width at that time is ΔV 34 Using the obtained value, the ohmic resistance (Ωcm 2 ) = {ΔV 12 (V) / 0.1(A / cm 2 ) + ΔV 34 (V) / 0.1(A / cm 2 )} / 2 Furthermore, by appropriately changing the target current density to be measured, the ohmic resistance at the target current density can be determined.

[0063] In the electrolysis system of the present invention, the amount of water transferred from the anode to the cathode is set to 10.0 mg / (cm ) from the viewpoint of reducing the amount of water present in the cathode catalyst layer and promoting the supply of the substance to be hydrogenated to the catalyst, thereby improving current efficiency. 2 min) or less, and 5.0 mg / (cm 2 min) or less, and 3.0 mg / (cm 2 ・min) or less, and 2.7 mg / (cm 2 From the viewpoint of maintaining the moisture content of the electrolyte membrane and reducing the resistance, it is preferable that the moisture content is 0.00 mg / (cm 2 ·min), and preferably exceeds 0.01 mg / (cm 2 ・min) or more, and 0.05 mg / (cm 2 ・minutes) or more is preferable.

[0064] The electrolysis system of the present invention is operated at a temperature of 0.6 A / cm after stabilizing the operating temperature, the liquid supply rate to the cathode chamber, and the liquid supply rate to the anode chamber. 2 The amount of water that migrates from the anode to the cathode, as measured by the method described in the Examples, can be measured.

[0065] The temperature when the electrolysis system of the present invention is used is not particularly limited as long as the hydrogenation reaction proceeds and the supplied water is maintained in a state of water vapor at a predetermined relative humidity. The temperature when the electrolysis system of the present invention is used is, for example, preferably 50 to 100°C, more preferably 70 to 90°C.

[0066] The electrolysis system of the present invention may be composed of a single electrolysis system basic unit 100 as shown in Fig. 1 , or may be composed of a repeating structure in which the electrolysis system basic unit 100 as shown in Fig. 1 is used as a repeating unit. An example of an electrolysis system composed of a repeating structure is an electrolysis system having a repeating structure in which electrolysis system basic units 100 are connected in series via bipolar plates (cathode-side bipolar plate 16a and anode-side bipolar plate 16b) such that, except for the electrolysis system basic units at the ends, the anode-side bipolar plate 16b also serves as the cathode-side bipolar plate 16a of the electrolysis system basic unit adjacent to it on the anode side.

[0067] An electrolysis system configured from a single electrolysis system basic unit 100 or a plurality of stacked electrolysis system basic units 100 as described above is operated by controlled input of the substance to be hydrogenated, the inert gas, the feed water 25, and DC power. For this purpose, a power control unit and a drive control unit (not shown) may be connected to the electrolysis system. The power control unit is, for example, a DC / DC converter that converts the output voltage of the power source into a predetermined voltage. The positive output terminal of the power control unit is connected to the anode-side bipolar plate 16b at one end of the electrolysis system. The negative output terminal of the power control unit is connected to the cathode-side bipolar plate 16a at the opposite end of the electrolysis system. As a result, a predetermined voltage is applied between the anode 17 and cathode 12 of the electrolysis system basic unit 100.

[0068] In the electrochemical system having the above-described structure, the reaction that occurs when toluene (TL) is used as an example of the substance to be hydrided is as follows. When toluene is used as the substance to be hydrided, the resulting organic hydride is methylcyclohexane (MCH). <Electrode reaction at the anode> 2H 2 O → O 2 + 4H ++4e - <Electrode reaction at the cathode> TL + 6H + + 6e - → MCH <Total reaction> 2TL + 6H 2 O → 2MCH + 3O 2

[0069] That is, the electrode reaction at the anode 17 and the electrode reaction at the cathode 12 proceed in parallel. Then, protons (H + ) is supplied to the cathode 12 via the solid polymer electrolyte membrane 11. The protons supplied to the cathode 12 are used to hydrogenate the substance to be hydrogenated at the cathode 12. As a result, toluene is hydrogenated to produce methylcyclohexane. Therefore, according to the electrolysis system of this embodiment, the electrolysis of water and the hydrogenation reaction of the substance to be hydrogenated can be carried out in one step. A similar electrode reaction proceeds even when a compound other than toluene is used as the substance to be hydrogenated.

[0070] (Method for producing a reduced substance) The electrolysis system of the present disclosure can be used for a method for producing a reduced substance (e.g., a hydride such as an organic hydride, or hydrogen). The method for producing a reduced substance of the present disclosure includes: (i) supplying water as water vapor in a gas inert to the anode of an electrolysis system including a proton-conductive electrolyte membrane, a cathode provided on one side of the electrolyte membrane and including a cathode catalyst for an electrochemical reaction involving protons, and an anode provided on the opposite side of the electrolyte membrane from the one side and including an anode catalyst for oxidizing water to produce protons, wherein the anode catalyst forms a porous layer and has a proton-conductive ionomer in part of the pores of the porous layer; (ii) in the case of producing a hydride, supplying a material to be hydrided, which will be a precursor of the hydride (e.g., an organic hydride), to the cathode of the electrolysis system; (iii) passing current through the electrolysis system; and (iv) simultaneously carrying out (i) to (iii) to reduce (e.g., hydrogenation, proton reduction) the substance to be reduced (e.g., substance to be hydrided, protons) by an electrochemical reaction at the cathode of the electrolysis system to generate a reduced product (e.g., a hydride such as an organic hydride, hydrogen) of the substance to be reduced (e.g., substance to be hydrided, protons).

[0071] The method for producing an organic hydride according to the present disclosure can be carried out by operating the electrolysis system of the present invention described above. The components of the electrolysis system, applicable combinations of a substance to be hydrided and a substance to be hydrided, conditions for supplying water vapor, and the like can be the same as those described for the electrolysis system of the present invention.

[0072] The present invention is not limited to the above-described embodiments, and various modifications such as design changes may be made based on the knowledge of those skilled in the art, and such modified embodiments may also be included within the scope of the present invention.

[0073] Examples of the present invention will be described below, but these examples are merely illustrative examples for suitably explaining the present invention and do not limit the present invention in any way.

[0074] (Fabrication of membrane-anode assembly) A catalyst ink for the anode catalyst layer was prepared by adding Nafion (registered trademark) dispersion DE521 (manufactured by DuPont) to powder of IrOx catalyst ELC-0110 (manufactured by Tanaka Kikinzoku Kogyo Co., Ltd.) The amount of Nafion (registered trademark) dispersion added was such that the mass of Nafion after drying was 22 wt % relative to the mass of the catalyst.

[0075] Furthermore, Nafion (registered trademark) 117 (thickness: 183 μm, manufactured by DuPont) was prepared as a solid polymer electrolyte membrane. The obtained catalyst ink was spray-coated onto one main surface of the solid polymer electrolyte membrane. The catalyst ink had an Ir mass of 1.0 mg / cm per electrode area. 2 The coating was then dried at 50°C to remove the solvent components in the catalyst ink, forming an anode consisting of a porous anode catalyst layer on the surface of the solid polymer electrolyte membrane, thereby obtaining a membrane-anode assembly. When the ratio of the carbon (002) diffraction intensity to the Ir oxide (110) diffraction intensity was measured by X-ray analysis of the anode catalyst layer, no carbon (002) peak was detected. The anode catalyst layer used in the examples did not contain a carbon material, and the carbon content was 0 wt %.

[0076] Furthermore, the At. % of the C1s, O1s, F1s, and S2p elements in the anode catalyst layer were measured using X-ray photoelectron spectroscopy (XPS) (ESCALAB250, manufactured by Thermo Fisher Scientific), and were found to be 30.21 At. %, 8.21 At. %, 60.24 At. %, and 1.34 At. % respectively. The excitation source used was mono. AlKα, 15 kV x 10 mA, with an analysis size of 1 mm (ellipse) and a photoelectron acceptance angle of 0°. A survey scan was performed from 0 to 1100 eV, and narrow scans were performed for C1s, O1s, F1s, and S2p. The relative element concentrations were calculated using the following formula: C j (%) = 100 x (I j / RSF j ) / Σ(I j / RSF j ) C j :Relative element concentration (atomic%) I jRSF: Area intensity of each spectrum calculated by linearizing the background (unit: cps eV) j : Relative sensitivity coefficients of Li 1s, O 1s, and C 1s (S 2p: 1.98, C 1s: 1.00, O 1s: 2.72, F 1s: 4.67)

[0077] (Preparation of cathode substrate / porous flow path) A cathode substrate / porous flow path was also prepared by supporting Pt particles on carbon paper. The Pt particles contained in the cathode substrate / porous flow path play a role in promoting the chemical reaction between hydrogen gas, a by-product at the cathode, and unreacted substances to be hydrided. First, H 2 PtCl 6 ・6H 2 A mixed solution was prepared by mixing 1-propanol with 1-propanol. 2 PtCl 6 ・6H 2 The amount of O added was set so that the amount of Pt supported on the carbon paper was 0.02 mg / cm 2 Carbon paper GDL38BC (manufactured by SGL Carbon Co., Ltd.) was immersed in the resulting mixed solution. The carbon paper was then completely dried under room temperature. Subsequently, 1 mg of NaBH 4 Carbon paper was immersed in the aqueous solution and subjected to reduction treatment for 2 hours. After the reduction treatment, the carbon paper was immersed in pure water for washing. Then, the carbon paper was dried to obtain a cathode substrate and porous flow path.

[0078] (Fabrication of Cathode and Fabrication of Cathode-Membrane-Anode Assembly) A PtRu / C catalyst (TEC61E54, manufactured by Tanaka Kikinzoku Kogyo K.K.), pure water, a 5 wt % Nafion (registered trademark) solution (manufactured by DuPont), and 1-propanol (manufactured by Wako Co., Ltd.) were placed in a ball mill container and mixed to prepare a catalyst ink for the cathode catalyst layer. The Nafion / carbon mass ratio of the catalyst ink was 0.8. This catalyst ink was applied to carbon paper GDL38BC (manufactured by SGL Carbon Co., Ltd.) using a bar coater so that the amount of precious metal (PtRu amount) was 0.5 mg / cm. 2The catalyst ink was then heated to 50°C to dry the solvent component in the catalyst ink, thereby obtaining a cathode catalyst layer. The obtained cathode substrate / porous flow path, cathode catalyst layer, and membrane-anode assembly were laminated in this order, with the cathode catalyst layer and the membrane side of the membrane-anode assembly (the surface not coated with the catalyst ink) facing each other, and hot-pressed at 120°C and 1 MPa for 3 minutes. This yielded a cathode-membrane-anode assembly.

[0079] (Fabrication of an organic hydride manufacturing apparatus) Cathode and anode bipolar plates, cathode and anode spacers, and an anode flow path structure were prepared. The cathode and anode bipolar plates were made of titanium. The cathode and anode spacers were made of Viton (trademark). The anode flow path structure was made of a Pt-plated Ti fiber sintered compact. The thickness of the anode flow path structure was 0.55 mm. The cathode bipolar plate, cathode-membrane-anode assembly (a laminate of a cathode substrate / porous flow path, a cathode catalyst layer, an electrolyte membrane, and an anode), anode flow path structure, and anode-side bipolar plate were stacked in this order, and the cathode-side spacer was positioned between the cathode-side bipolar plate and the electrolyte membrane and in close contact with the cathode (cathode substrate / porous flow path and cathode catalyst layer), and the anode-side spacer was positioned between the electrolyte membrane and the anode-side bipolar plate and in close contact with the anode (anode catalyst layer) and anode flow path structure. The components were then arranged and fastened with bolts and nuts. The elastic force of the anode flow path structure pressed the layers together, creating a state in which the layers were in close contact with each other. These stacks were assembled under a pressure of 0.93 MPa. This resulted in an organic hydride production apparatus (electrolytic cell, electrolysis system) having each membrane electrode assembly. The effective electrode area of ​​the organic hydride production apparatus was 16 cm. 2 It was decided.

[0080] Example 1 Using the above-described organic hydride production apparatus, a supply path for the material to be hydrided was connected to the cathode-side inlet for the material to be hydrided. A hydride discharge path was connected to the cathode-side hydride outlet. A humidified air supply path was connected to the anode-side humidified gas inlet. A humidified air discharge path was connected to the anode-side humidified gas outlet. The anode-side humidified air supply path was covered with a heat insulator and heated with a ribbon heater to prevent condensation due to temperature drop. 10% v / v (relative to methylcyclohexane) toluene was circulated at a flow rate of 5 mL / min as an initial cathode fluid (liquid containing the material to be hydrided) through the cathode chamber (the space housing the cathode). Humidified air at 80°C and 100% RH was circulated through the anode chamber at a flow rate of 0.8 L / min. The temperature of the electrolytic cell was adjusted to 80°C using a rod-shaped heater.

[0081]

[0082] (IV Measurement) The organic hydride production apparatus was connected to an electrochemical property evaluation apparatus (VSP300, manufactured by Biologic), and an electrolytic reduction reaction (electrolytic hydrogenation reaction) of toluene was carried out under the conditions shown in Table 1. The current density was 0.1 A / cm 2 The potential was measured at each current density within a range in which the potential did not exceed 2.2 V. 2 The potentials measured are shown in Table 2.

[0083] (Current Efficiency Measurement) A hydrogen recovery tube made of PP and approximately 120 cm long was attached to the end of the discharge path of the cathode-side hydride outlet, branched by a three-way cock. The cathode solution was allowed to flow without applying voltage, filling the hydrogen recovery tube. The weight of the solution in the hydrogen recovery tube was measured as the initial weight. Next, electrolysis was started at a predetermined current density, and electrolysis was performed for a certain period of time (electrolysis time (sec)), with the time when the cathode solution began to be collected in the hydrogen recovery tube filled with the cathode solution being designated as 0 (sec). The electrolysis time was adjusted so that the hydrogen recovery tube was not completely filled with hydrogen, and the generated hydrogen was recovered. The weight of the solution in the hydrogen recovery tube was measured as the post-electrolysis weight (g). It was confirmed that the cathode solution in the hydrogen recovery tube had cooled to room temperature. The volume of generated hydrogen was calculated from the initial weight (g) and post-electrolysis weight (g) according to the following formula, and the current efficiency was determined. At this time, it was assumed that no reactions other than the electrolytic hydrogenation reaction of toluene and the hydrogen generation reaction were occurring at the cathode. The cathode liquid density was 0.77915 (g / cm 3 ) was calculated. F was calculated as 96485 (sec A / mol). Hydrogen volume (cm 3 ) = (initial weight (g) - weight after electrolysis (g)) / cathode solution density (g / cm 3 ) Amount of hydrogen (mol) = Hydrogen volume (cm 3 ) × 101.3 (kPa) / 8.31 (kPa L / K mol) / temperature (K) Current efficiency (%) = {1 - amount of hydrogen (mol) × 2 × F (A sec / mol) / [(electrolysis current density (A / cm 2 ) × effective electrode area (cm 2 ) x electrolysis time (sec)] x 100

[0084] (Ohmic Resistance Measurement) The organic hydride production apparatus was connected to an electrochemical property evaluation apparatus (VSP300, manufactured by Biologic), and after adjusting the conditions as shown in Table 1, a voltage of 0.60 A / cm 2 After holding at 40°C for 30 seconds, impedance measurement was carried out under the following conditions. From the obtained Nyquist plot, the ohmic resistance (Ω cm) was calculated by multiplying the intersection of the plot on the high frequency side with the real axis by the electrode area. 2) was calculated. Current density: 0.60 A / cm 2 Amplitude: 40mA Frequency: 100.0kHz to 10.0mHz Number of measurement points: 6 / decade

[0085] (Measurement of Water Transfer Amount) The organic hydride production apparatus was connected to an electrochemical property evaluation apparatus (VSP300, manufactured by Biologic Co., Ltd.), and after adjusting the conditions to those shown in Table 1, a current of 0.60 A / cm 2 The electrolytic reduction reaction of toluene was carried out at 0.05 A / cm 2. At this time, in order to collect the migrated water discharged from the cathode chamber without leaving it on the vessel wall, a Teflon (registered trademark) tube was connected to the cathode chamber outlet, and the cathode solution was collected in a PP bottle. The time when collection began in an empty PP bottle was set to 0 minutes, and the cathode solution was collected after 30 minutes of electrolysis. Separated migrated water was confirmed at the bottom of the bottle. The entire amount of migrated water was collected using a PP dropper in an empty PP test tube whose weight had been measured in advance, and the weight of the collected migrated water (mg) was measured. Note that the electrolysis time was adjusted so that the amount of migrated water that could be collected exceeded 1 g to ensure accurate measurement. 0.60 A / cm 2 2 The amount of water transferred was measured by extending the electrolysis time at current densities other than 1000 kJ / cm. The results are shown in Table 2 and Figure 4. 2 min) = recovered migrated water (mg) / (electrode effective area (cm 2 )×electrolysis time (min))

[0086] *1 0.4A / cm 2 Measurement value at *2 0.1 to 0.4 A / cm 2 Reference value calculated from the measurement results

[0087] (Examples 2 to 8) The humidification conditions for the anode-side supplied water and the anode-side humidified air flow rate were set as shown in Table 1, and the above-mentioned characteristic evaluation was carried out in the same manner as in Example 1. The results are shown in Table 2 and Figures 2 to 4. In Examples 7 and 8, a small amount of condensed water was discharged from the anode-side outlet.

[0088] Comparative Example 1 Using the above-described organic hydride production apparatus, a supply path for the material to be hydrided was connected to the cathode-side inlet for the material to be hydrided. A hydride discharge path was connected to the cathode-side hydride outlet. A water supply path was connected to the anode-side humidified gas inlet. A water discharge path was connected to the anode-side humidified gas outlet. 10% v / v (relative to methylcyclohexane) toluene was circulated through the cathode chamber as an initial cathode fluid (liquid containing the material to be hydrided) at a flow rate of 5 mL / min. Water heated to 60°C was circulated through the anode chamber at a rate of 5 mL / min. The temperature of the electrolytic cell was adjusted to 80°C using a rod-shaped heater. The results are shown in Table 2 and Figures 2 to 4.

[0089] Comparative Example 2 The same procedure as in Comparative Example 1 was carried out, except that the water supplied to the anode chamber was heated to 80° C. and circulated at a rate of 10 mL / min. The results are shown in Table 2 and Figures 2 to 4.

[0090] Comparative Example 3 The same procedure as in Example 1 was carried out, except that the anode-side humidified air flow rate was 0.5 L / min. The electrolyte membrane was not sufficiently humidified, the voltage was high, and the current was 0.4 A / cm 2 Therefore, the ohmic resistance was measured at 0.4 A / cm 2 The ohmic resistance measured at 1000 kJ / s is shown in Table 2. The resistance was high, making stable electrolysis impossible, and the amount of water transferred was very small, so the amount of water transferred was not measured. The results are shown in Table 2 and Figures 2 and 3.

[0091] Comparative Example 4 The same procedure as in Comparative Example 1 was carried out, except that the water supplied to the anode chamber was a 1 M diluted aqueous sulfuric acid solution heated to 60° C. The potential was high, 0.4 A / cm 2 Therefore, the ohmic resistance was measured at 0.4 A / cm 2 The ohmic resistance measured at 0.1 A / cm is shown in Table 2. Although the potential was high, a large amount of water was transferred. 2 ~0.4 A / cm 2 The amount of migrated water was measured at 0.1 A / cm. Since the amount of migrated water increases in proportion to the current density, 2 ~0.4 A / cm 2 0.6 A / cm2 The amount of water transferred at this time is shown as a reference value in Table 2. The results are shown in Table 2 and Figures 2 to 4.

[0092] (Evaluation of the Relationship between Anode-Side Supply Method and Transferred Water Amount) Figure 4 shows the relationship between the amount of transferred water discharged from the hydride outlet and the current density (i) (comparison of Examples 1 to 6 and Comparative Examples 1, 2, and 4). It was confirmed that the amount of transferred water was reduced to less than one-third when using the humidified air anode supply method compared to when using water anode supply method. This can be understood as the fact that, compared to the water anode supply method, the humidified air anode supply method supplies the minimum amount of water while ensuring the amount of water used in the oxygen generation reaction at the anode and swelling of the solid polymer electrolyte membrane, resulting in a reduced amount of water transferred to the cathode.

[0093] (Evaluation of the relationship between anode-side supply method and current efficiency) Figure 2 shows the relationship between current efficiency (ε) and current density (i). While the current efficiency significantly decreased when water was supplied to the anode, the example in which the electrolyte membrane swelling was appropriately adjusted when humidified air was supplied to the anode significantly suppressed the decrease in current efficiency. The decrease in current efficiency is due to the fact that migration water accumulated in the cathode catalyst layer inhibits toluene diffusion to the cathode catalyst, resulting in hydrogen generation. The improvement in current efficiency when humidified air is supplied to the anode is thought to be due to the improved catalyst utilization rate resulting from the reduction in water migration from the anode to the cathode, which reduces the amount of accumulated water in the cathode catalyst layer.

[0094] (Evaluation of the relationship between the amount of transferred water and the ohmic resistance) 2 This figure shows the relationship between the amount of transferred water measured in the anode supply method using water and an aqueous sulfuric acid solution, and the ohmic resistance. The amount of transferred water is high when the anode supply method uses water and an aqueous sulfuric acid solution. While the amount of transferred water can be reduced to some extent by lowering the temperature and adding sulfuric acid, it does not reach the range of transferred water required to improve current efficiency. The amount of transferred water can be significantly reduced when the anode supply method uses humidified air compared to the water supply method. When the amount of humidified air supplied is insufficient, the ohmic resistance increases due to a lack of moisture in the electrolyte membrane, but by increasing the supply amount, the ohmic resistance can be reduced.

[0095] According to the present invention, an electrolysis system is provided in which the current efficiency of the electrolytic hydrogenation reaction is improved by suppressing the amount of water that migrates to the cathode in association with protons that migrate from the anode to the cathode during electrolysis, and at the same time, supplying the necessary water to the electrolyte membrane to reduce the resistance of the electrolyte membrane.

[0096] REFERENCE SIGNS LIST 11 Solid polymer electrolyte membrane 12 Cathode 12a Cathode catalyst layer 12b Cathode substrate and porous flow path 13 Inlet for material to be hydrided 14 Outlet for hydrided material 15 Cathode side spacer 16a Cathode side bipolar plate 16b Anode side bipolar plate 17 Anode 17a Anode catalyst layer 17b Anode substrate 18 Anode flow path structure 19 Anode chamber 20 Inlet for humidified gas 21 Outlet for humidified gas 22 Anode side spacer 23 Humidifier body 24 Inert gas inlet 25 Feed water 100 Basic unit of electrolysis system

Claims

1. An electrolysis system comprising: an electrolyte membrane having proton conductivity; a cathode provided on one side of the electrolyte membrane and having a cathode catalyst layer containing a cathode catalyst for an electrochemical reaction involving protons; an anode provided on the opposite side of the electrolyte membrane and having an anode catalyst layer containing an anode catalyst for oxidizing water to generate protons; and a structure for supplying water vapor to the anode, wherein a proton-conductive ionomer is contained in a portion of the anode catalyst layer, and the anode catalyst layer has an X-ray analysis ratio of the carbon (002) diffraction peak intensity to the Ir oxide (110) diffraction peak intensity of 0.10 or less and a current density of 0.6 A / cm 2 The ohmic resistance measured at is 0.400 Ω cm 2 Below is an electrolysis system.

2. 0.6A / cm 2 The amount of water transferred from the anode to the cathode, measured by 2 min), 10.0 mg / (cm 2 2. The electrolysis system according to claim 1, wherein the electrolysis time is 10 min or less.

3. 0.6A / cm 2 The amount of water transferred from the anode to the cathode, measured by 2 min), 5.0 mg / (cm 2 3. The electrolysis system according to claim 1 or 2, wherein the electrolysis time is 10 min or less.

4. The electrolysis system according to claim 1 or 2, wherein the structure for supplying water vapor to the anode further comprises a mechanism for preventing condensation of the vapor.

5. The electrolysis system according to claim 1 or 2, wherein the anode catalyst layer forms a porous layer.

6. The electrolysis system according to claim 1 or 2, wherein the water vapor supplied to the anode is water vapor in a gas inert to the electrochemical reaction.

7. The electrolysis system according to claim 1 or 2, wherein the water vapor supplied to the anode is water vapor in the air.

8. The electrolysis system according to claim 1 or 2, wherein the relative humidity of the water vapor at the anode supplied by the structure for supplying water as water vapor can be controlled to any value between 70% and 100%.

9. The electrolysis system according to claim 6, wherein the relative humidity at the anode of the water vapor supplied by the structure for supplying water as water vapor can be controlled to any value between 70% and 100%.

10. The electrolysis system according to claim 1 or 2, further comprising a structure for supplying an aromatic compound to the cathode as a reaction substrate for obtaining a target product by a hydrogenation reaction.

11. The electrolysis system of claim 10, wherein the aromatic compound is toluene.

12. The electrolyte membrane and the anode catalyst layer form a membrane electrode assembly, and the mass of the anode catalyst in the anode catalyst layer is 0.1 mg / cm per electrode area. 2 5.0mg / cm or more 2 3. The electrolysis system according to claim 1 or 2, wherein:

13. The electrolyte membrane and the cathode catalyst layer form a membrane electrode assembly, and the mass of the cathode catalyst in the cathode catalyst layer is 0.1 mg / cm per electrode area. 2 5.0mg / cm or more 2 3. The electrolysis system according to claim 1 or 2, wherein:

14. A method for operating the electrolysis system according to claim 1 or 2, comprising controlling the relative humidity of water vapor in the anode to an arbitrary value between 70% and 100%.