Coating composition for laminated steel sheet
Patent Information
- Application Number
- MYPI2026001707
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-09-26
- Filing Date
- 2024-09-26
- Publication Date
- 2025-03-26
AI Technical Summary
Conventional methods for manufacturing laminated steel sheets using magnetic steel sheets with adhesive coatings face challenges in achieving high adhesive strength under high temperature conditions while maintaining excellent coatability, leading to issues with magnetic property degradation and mechanical rigidity, noise, and vibration.
A coating composition for laminated steel sheets comprising (meth)acrylic resin particles A with specific structural units and a water-soluble (meth)acrylic resin B, formulated to provide high adhesive strength and coatability, utilizing a balanced ratio of these resins to enhance cohesive strength and wettability, thereby forming a coating film that maintains integrity under high temperature bonding conditions.
The composition achieves high adhesive strength and excellent coatability, reducing magnetic property degradation and noise/vibration issues, while eliminating the need for a curing agent, thus ensuring a long pot life and improved bonding efficiency.
Abstract
Description
Coating composition for laminated steel sheets
[0001] The present disclosure relates to coating compositions for steel laminates.
[0002] High efficiency, compact size, and high output are important for motors, so motor core materials must have high magnetic permeability and low iron loss, and core processing can be problematic due to the degradation of core magnetic properties. Furthermore, low noise and low vibration from motors are becoming increasingly important from the perspective of protecting the living environment, and high-precision positioning control is required for motors. Motor cores are generally made of laminated steel sheets, which are made by laminating electromagnetic steel sheets.
[0003] Conventionally, methods such as welding, caulking, and bolting have been used to secure magnetic steel sheets together when manufacturing laminated steel sheets. However, these methods result in degradation of magnetic properties. Furthermore, laminated steel sheets manufactured using these methods lack sufficient mechanical rigidity, raising concerns about noise and vibration. Therefore, in recent years, a method has been adopted for manufacturing laminated steel sheets using magnetic steel sheets on whose surfaces a coating that exhibits adhesive properties when heated and pressed (also known as "adhesive-coated magnetic steel sheets") has been formed. In this method, punched or sheared magnetic steel sheets with adhesive coatings are stacked and then bonded together by heating and pressing. Compared to laminated steel sheets manufactured by welding or other methods to fix magnetic steel sheets together, laminated steel sheets manufactured using adhesive-coated magnetic steel sheets tend to be less susceptible to deterioration in magnetic properties due to the process of fixing, and also have higher core rigidity, making them less susceptible to noise and vibration problems (see Kaido Chikara, Takeda Kazutoshi, Wakisaka Takeaki, Mizogami Masato, "On the Properties of Bonded Magnetic Steel Sheet Cores," Journal of Electrical Engineering D, Vol. 119, No. 7, pp. 1010-1015, 1999).
[0004] An example of an adhesive coated electrical steel sheet is an electrical steel sheet having an insulating coating on the surface that exhibits adhesive properties when heated and / or pressed, wherein the coating is a mixture of a dispersed epoxy resin or modified epoxy resin having a glass transition point (Tg) of 80°C to 150°C, an epoxy resin curing agent, and a particulate polymer having a particle size of 0.01 μm to 0.5 μm (see WO 2004 / 070080).
[0005] When manufacturing laminated steel sheets using adhesive-coated electrical steel sheets, a coating agent for forming an adhesive coating (also referred to as a "coating agent for forming an adhesive coating") is first applied to the surface of the electrical steel sheet, followed by drying at high temperature to produce an adhesive-coated electrical steel sheet. The produced adhesive-coated electrical steel sheets are then stacked and further bonded by hot pressing at high temperature. Therefore, the adhesive-coating agent is required to form a coating film that exhibits high adhesive strength under the high-temperature conditions used when bonding the laminated adhesive-coated electrical steel sheets. Furthermore, the adhesive coating is required to function not only as an adhesive for bonding the laminated electrical steel sheets but also as an insulating coating formed on the surface of the electrical steel sheet. In general, insulating coatings are required to have insulating properties and corrosion resistance. Therefore, the adhesive-coating agent is required to form an adhesive coating that is resistant to cissing and cracking, in other words, to have excellent coatability. When the application properties of a coating agent for forming an adhesive film are excellent, the adhesive film formed has improved uniformity, making it less likely to lose its insulating properties and corrosion resistance, and improving its adhesive strength can also be expected. In order to increase the adhesive strength of the adhesive film, it is necessary to increase the cohesive strength of the resin used in the coating agent. However, increasing the cohesive strength of the resin can reduce the wettability required for the application properties of the coating agent. Therefore, increasing the adhesive strength of the adhesive film and improving the application properties of the coating agent for forming the adhesive film are in a trade-off relationship, and it has been difficult to achieve both.
[0006] An object of one embodiment of the present disclosure is to provide a coating composition for laminated steel sheets, which is a composition for coating the surface of an electrical steel sheet used in the production of laminated steel sheets, and which is capable of forming a coating film that exhibits high adhesive strength under the high-temperature conditions used when bonding electrical steel sheets together, and which has excellent coatability.
[0007] Specific means for solving the problems include the following aspects. <1> A coating composition for a laminated steel sheet, comprising: (meth)acrylic resin particles A containing structural units derived from a monomer having a carboxy group in an amount of 1% by mass or more and less than 20% by mass, based on all structural units, and structural units derived from a monomer having a self-crosslinking group in an amount of 0.1% by mass or more and 7% by mass or less, based on all structural units, and having a glass transition temperature of 55°C or higher; a water-soluble (meth)acrylic resin B; and water, wherein the ratio of the mass content of the (meth)acrylic resin particles A to the mass content of the water-soluble (meth)acrylic resin B is 95 / 5 to 85 / 15. <2> The coating composition for a laminated steel sheet according to <1>, wherein the water-soluble (meth)acrylic resin B contains structural units derived from a monomer having a self-crosslinking group. <3> The coating composition for a laminated steel sheet according to <1> or <2>, wherein the water-soluble (meth)acrylic resin B contains structural units derived from a monomer having a hydroxyl group. <4> The coating composition for laminated steel sheets according to any one of <1> to <3>, wherein the (meth)acrylic resin particles A have an average primary particle size of 250 nm to 450 nm. <5> The coating composition for laminated steel sheets according to any one of <1> to <4>, wherein the monomer having a self-crosslinking group in the (meth)acrylic resin particles A is at least one selected from the group consisting of N-methylolacrylamide (NMAM), N-butylolacrylamide (NBMA), hydroxyethylacrylamide (HEAA), and glycidyl methacrylate (GMA). <6> The coating composition for laminated steel sheets according to any one of <2> to <5>, wherein the content of structural units derived from the monomer having a self-crosslinking group in the water-soluble (meth)acrylic resin B is 0.1 mass % to 10.0 mass % relative to the total structural units of the water-soluble (meth)acrylic resin B. <7> The coating composition for laminated steel sheet according to any one of <3> to <6>, wherein a content of structural units derived from the monomer having a hydroxyl group in the water-soluble (meth)acrylic resin B is 5% by mass to 30% by mass relative to all structural units of the water-soluble (meth)acrylic resin B.
[0008] According to one embodiment of the present disclosure, there is provided a coating composition for laminated steel sheets, which is a composition for coating the surface of an electrical steel sheet used in the production of laminated steel sheets, and which is capable of forming a coating film that exhibits high adhesive strength under the high-temperature conditions used when bonding electrical steel sheets together, and which has excellent coatability.
[0009] The coating composition for laminated steel sheets of the present disclosure will be described in detail below. The following description of the requirements may be based on a representative embodiment of the present disclosure, but the present disclosure is not limited to such an embodiment and can be implemented with appropriate modifications within the scope of the present disclosure.
[0010] In the present disclosure, a numerical range indicated using "to" means a range that includes the numerical values before and after "to" as the lower and upper limits, respectively. In the numerical ranges described in stages in the present disclosure, the upper or lower limit described in a certain numerical range may be replaced with the upper or lower limit of another numerical range described in stages. Furthermore, in the numerical ranges described in the present disclosure, the upper or lower limit described in a certain numerical range may be replaced with a value shown in the examples.
[0011] In the present disclosure, a combination of two or more preferred aspects is a more preferred aspect.
[0012] In the present disclosure, when a plurality of substances corresponding to each component are present in the coating composition for laminated steel sheets, the amount of each component in the coating composition for laminated steel sheets means the total amount of the plurality of substances present in the coating composition for laminated steel sheets, unless otherwise specified.
[0013] In the present disclosure, the term "(meth)acrylic monomer" refers to a monomer having a (meth)acryloyl group. In the present disclosure, the term "(meth)acrylic resin" refers to a resin that contains structural units derived from a (meth)acrylic monomer and in which the proportion of structural units derived from the (meth)acrylic monomer is 50 mass% or more.
[0014] In the present disclosure, "(meth)acrylic" is a term that encompasses both "acrylic" and "methacrylic," "(meth)acrylate" is a term that encompasses both "acrylate" and "methacrylate," "(meth)acryloyl" is a term that encompasses both "acryloyl" and "methacryloyl," and "(meth)acrylamide" is a term that encompasses both "acrylamide" and "methacrylamide."
[0015] In this disclosure, "n-" means normal, "i-" means iso, "s-" means secondary, and "t-" means tertiary.
[0016] In the present disclosure, "% by mass" and "% by weight" are synonymous, and "parts by mass" and "parts by weight" are synonymous.
[0017] In the present disclosure, the term "process" includes not only an independent process but also a process that cannot be clearly distinguished from other processes, as long as the intended purpose of the process is achieved.
[0018] [Coating Composition for Laminated Steel Sheets] The coating composition for laminated steel sheets (hereinafter also referred to as the "coating composition") of the present disclosure contains structural units derived from monomers having carboxy groups in a proportion of 1% by mass or more but less than 20% by mass, based on all structural units, and structural units derived from monomers having self-crosslinking groups in a proportion of 0.1% by mass or more but less than 7% by mass, based on all structural units, and contains (meth)acrylic resin particles A having a glass transition temperature of 55°C or higher, a water-soluble (meth)acrylic resin B, and water, wherein the ratio of the mass content of the (meth)acrylic resin particles A to the mass content of the water-soluble (meth)acrylic resin B is 95 / 5 to 85 / 15. The coating composition of the present disclosure is a composition for coating the surface of an electrical steel sheet used in the production of laminated steel sheets, and is capable of exhibiting high adhesive strength at or above a specific temperature.
[0019] Generally, increasing the cohesive strength of the resin contained in the coating agent to improve the adhesive strength of the coating film can reduce the wettability required for the coatability of the coating agent. In contrast, the coating composition of the present disclosure contains (meth)acrylic resin particles A, which ensure cohesive strength, and water-soluble (meth)acrylic resin B, which ensures wettability, in specific proportions, thereby achieving both high adhesive strength of the coating film and excellent coatability of the coating composition. The coating composition of the present disclosure contains (meth)acrylic resin particles A, which have high cohesive strength and a specific proportion of carboxy groups and self-crosslinking groups that contribute to crosslinking, and therefore can form a coating film that exhibits high adhesive strength. Furthermore, in the coating composition of the present disclosure, the (meth)acrylic resin particles A have self-crosslinking groups that exhibit self-crosslinking properties at a specific temperature or higher, and therefore the coating film can exhibit adhesive strength under high-temperature conditions when bonding electrical steel sheets together. Furthermore, the coating composition of the present disclosure contains a combination of (meth)acrylic resin particles A and water-soluble (meth)acrylic resin B, which improves wettability with respect to electrical steel sheets and increases the adhesive area with the electrical steel sheets, compared to a composition containing only (meth)acrylic resin particles A. Thus, the coating composition of the present disclosure can form a coating film that exhibits high adhesive strength under the high-temperature conditions used when bonding electrical steel sheets together, and has excellent coatability.
[0020] Furthermore, the coating composition of the present disclosure has the advantage of not requiring a curing agent to develop adhesive strength and having a long pot life. For example, the treatment liquid (so-called coating agent) used in the production of adhesive surface-coated electrical steel sheets described in International Publication No. 2004 / 070080 uses an epoxy resin, and therefore requires the incorporation of a curing agent to develop adhesive strength. While coating agents containing a curing agent tend to have a shorter pot life, the coating composition of the present disclosure is less susceptible to the reduction in pot life caused by the incorporation of a curing agent.
[0021] In the present disclosure, "(meth)acrylic resin particles A that contain structural units derived from monomers having a carboxy group in a proportion of 1% by mass or more and less than 20% by mass, relative to all structural units, and structural units derived from monomers having a self-crosslinking group in a proportion of 0.1% by mass or more and 7% by mass or less, relative to all structural units, and that have a glass transition temperature of 55°C or higher" are also referred to as "specific (meth)acrylic resin particles A."
[0022] [Specific (meth)acrylic resin particles A] The coating composition of the present disclosure comprises (meth)acrylic resin particles A which contain structural units derived from monomers having a carboxy group in a proportion of 1% by mass or more and less than 20% by mass, relative to all structural units, and structural units derived from monomers having a self-crosslinking group in a proportion of 0.1% by mass or more and 7% by mass or less, relative to all structural units, and which have a glass transition temperature of 55° C. or more. The coating composition of the present disclosure may contain only one type of specific (meth)acrylic resin particles A, or may contain two or more types. In the coating composition of the present disclosure, the specific (meth)acrylic resin particles A are present in a dispersed state in a medium containing water.
[0023] <Constituent units derived from monomers having a carboxy group> The specific (meth)acrylic resin particles A contain constituent units derived from monomers having a carboxy group in a proportion of 1% by mass or more and less than 20% by mass of all constituent units. In the present disclosure, "constituent units derived from monomers having a carboxy group" means constituent units formed by addition polymerization of monomers having a carboxy group.
[0024] Examples of the monomer having a carboxy group include a monomer having at least one carboxy group and an ethylenically unsaturated group in one molecule. The ethylenically unsaturated group is not particularly limited, and examples thereof include a vinyl group, an allyl group, a vinylphenyl group, a (meth)acrylamide group, and a (meth)acryloyl group. The ethylenically unsaturated group is preferably a (meth)acryloyl group.
[0025] Specific examples of monomers having a carboxy group include (meth)acrylic acid, crotonic acid, maleic acid, fumaric acid, itaconic acid, glutaconic acid, citraconic acid, ω-carboxy-polycaprolactone mono(meth)acrylate [e.g., ω-carboxy-polycaprolactone (n≒2) monoacrylate], and succinic acid derivatives (e.g., 2-acryloyloxyethyl-succinic acid). The monomer having a carboxy group preferably includes a (meth)acrylic monomer having a carboxy group, and more preferably a (meth)acrylic monomer having a carboxy group. The (meth)acrylic monomer having a carboxy group is preferably (meth)acrylic acid, and more preferably methacrylic acid.
[0026] The specific (meth)acrylic resin particles A may contain only one type of structural unit derived from a monomer having a carboxy group, or may contain two or more types.
[0027] The content of structural units derived from monomers having a carboxy group in the specific (meth)acrylic resin particles A is 1% by mass or more and less than 20% by mass, relative to the total structural units of the specific (meth)acrylic resin particles A. When the content of structural units derived from monomers having a carboxy group in the specific (meth)acrylic resin particles A is 1% by mass or more, relative to the total structural units of the specific (meth)acrylic resin particles A, a coating film exhibiting high adhesive strength under high-temperature conditions when bonding magnetic steel sheets together tends to be formed. From this perspective, the content of structural units derived from monomers having a carboxy group in the specific (meth)acrylic resin particles A is preferably 3% by mass or more, more preferably 5% by mass or more, even more preferably 8% by mass or more, and particularly preferably 10% by mass or more, relative to the total structural units of the specific (meth)acrylic resin particles A. When the content of structural units derived from monomers having a carboxy group in the specific (meth)acrylic resin particles A is less than 20% by mass relative to the total structural units of the specific (meth)acrylic resin particles A, a coating film exhibiting high adhesive strength under high-temperature conditions when bonding magnetic steel sheets tends to be formed. From this perspective, the content of structural units derived from monomers having a carboxy group in the specific (meth)acrylic resin particles A is preferably 18% by mass or less, more preferably 15% by mass or less, relative to the total structural units of the specific (meth)acrylic resin particles A. In one embodiment, the content of structural units derived from monomers having a carboxy group in the specific (meth)acrylic resin particles A may be in the range of 5% by mass or more and less than 20% by mass, 8% by mass or more and less than 20% by mass, 10% by mass or more and less than 20% by mass, 8% by mass or more and less than 18% by mass, or 10% by mass or more and less than 15% by mass.
[0028] <Constituent Units Derived from Monomers Having Self-Crosslinking Groups> The specific (meth)acrylic resin particles A contain constituent units derived from monomers having self-crosslinking groups in a proportion of 0.1% by mass or more and 7% by mass or less of all constituent units. In the present disclosure, the term "constituent units derived from monomers having self-crosslinking groups" refers to constituent units formed by addition polymerization of monomers having self-crosslinking groups.
[0029] In the present disclosure, the term "self-crosslinking" refers to the property of being able to crosslink even in the absence of a crosslinking agent.
[0030] The self-crosslinking group in the present disclosure can exhibit self-crosslinking properties by heating. The temperature at which the self-crosslinking group exhibits self-crosslinking properties varies depending on the type of self-crosslinking group. The self-crosslinking group is unlikely to exhibit self-crosslinking properties at the temperature at which a coating composition is applied to the surface of an electrical steel sheet and dried, and it is sufficient for the self-crosslinking group to exhibit self-crosslinking properties at the temperature at which the electrical steel sheets are bonded together, and the temperature at which the self-crosslinking group exhibits self-crosslinking properties is not particularly limited.
[0031] Specific examples of the self-crosslinking group include an N-methylol group, an N-butyrol group, a glycidyl group, and an alkoxymethylamide group. The self-crosslinking group is preferably at least one selected from the group consisting of an N-methylol group, an N-butyrol group, and a glycidyl group.
[0032] Specific examples of monomers having a self-crosslinking group include N-hydroxyalkyl(meth)acrylamide, N,N-dihydroxyalkyl(meth)acrylamide, glycidyl(meth)acrylate, and N-alkoxymethyl(meth)acrylamide. Examples of N-hydroxyalkyl(meth)acrylamides include N-methylolacrylamide (NMAM), N-butyrolacrylamide (NBMA), and hydroxyethylacrylamide (HEAA). Examples of N,N-dihydroxyalkyl(meth)acrylamides include dimethylol(meth)acrylamide. Examples of N-alkoxymethyl(meth)acrylamides include N-methoxymethyl(meth)acrylamide, N-ethoxymethyl(meth)acrylamide, and N-butoxymethyl(meth)acrylamide. The monomer having a self-crosslinking group is preferably at least one selected from the group consisting of N-methylolacrylamide (NMAM), N-butylolacrylamide (NBMA), hydroxyethylacrylamide (HEAA), and glycidyl methacrylate (GMA), more preferably includes hydroxyethylacrylamide (HEAA), and even more preferably is hydroxyethylacrylamide (HEAA).
[0033] The specific (meth)acrylic resin particles A may contain only one type of structural unit derived from a monomer having a self-crosslinking group, or may contain two or more types.
[0034] The content of structural units derived from monomers having self-crosslinking groups in the specific (meth)acrylic resin particles A is 0.1% by mass or more and 7% by mass or less, relative to the total structural units of the specific (meth)acrylic resin particles A. The content of structural units derived from monomers having self-crosslinking groups in the specific (meth)acrylic resin particles A being 0.1% by mass or more, relative to the total structural units of the specific (meth)acrylic resin particles A, means that the specific (meth)acrylic resin particles A actively contain structural units derived from monomers having self-crosslinking groups. The content of structural units derived from monomers having self-crosslinking groups in the specific (meth)acrylic resin particles A, relative to the total structural units of the specific (meth)acrylic resin particles A, is preferably 0.5% by mass or more, more preferably 1% by mass or more, and even more preferably 1.5% by mass or more. When the content of structural units derived from monomers having self-crosslinking groups in the specific (meth)acrylic resin particles A is 7% by mass or less relative to the total structural units of the specific (meth)acrylic resin particles A, a coating film exhibiting high adhesive strength under high-temperature conditions when bonding magnetic steel sheets tends to be formed. From this perspective, the content of structural units derived from monomers having self-crosslinking groups in the specific (meth)acrylic resin particles A is preferably 6% by mass or less, more preferably 5% by mass or less, relative to the total structural units of the specific (meth)acrylic resin particles A. In one embodiment, the content of structural units derived from monomers having self-crosslinking groups in the specific (meth)acrylic resin particles A may be in the range of 0.1% by mass or more to 6% by mass or less, 0.1% by mass or more to 5% by mass or less, 1% by mass or more to 7% by mass or less, 1.5% by mass or more to 6% by mass or less, or 1.9% by mass or more to 5% by mass or less.
[0035] <Constituent Units Derived from (Meth)acrylic Acid Alkyl Ester Monomers> The specific (meth)acrylic resin particles A preferably contain constituent units derived from (meth)acrylic acid alkyl ester monomers. In the present disclosure, the term "constituent units derived from (meth)acrylic acid alkyl ester monomers" refers to constituent units formed by addition polymerization of (meth)acrylic acid alkyl ester monomers. Note that the "(meth)acrylic acid alkyl ester monomer" in the specific (meth)acrylic resin particles A does not include monomers corresponding to monomers having a carboxy group or monomers corresponding to monomers having a self-crosslinking group.
[0036] The type of (meth)acrylic acid alkyl ester monomer is not particularly limited. The (meth)acrylic acid alkyl ester monomer may be an acrylic acid alkyl ester monomer or a methacrylic acid alkyl ester monomer. The alkyl group contained in the (meth)acrylic acid alkyl ester monomer may be unsubstituted or may have a substituent (excluding a carboxy group, a self-crosslinkable group, and a hydroxyl group), but is preferably unsubstituted. The alkyl group contained in the (meth)acrylic acid alkyl ester monomer may be linear, branched, or cyclic. The number of carbon atoms in the alkyl group contained in the (meth)acrylic acid alkyl ester monomer is, for example, preferably 1 to 18, more preferably 1 to 12, and even more preferably 1 to 8.
[0037] Specific examples of the (meth)acrylic acid alkyl ester monomer include methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, i-butyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, n-octyl (meth)acrylate, i-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-nonyl (meth)acrylate, i-nonyl (meth)acrylate, n-decyl (meth)acrylate, stearyl (meth)acrylate, lauryl (meth)acrylate, cyclohexyl (meth)acrylate, and isobornyl (meth)acrylate. The (meth)acrylic acid alkyl ester monomer preferably contains at least one selected from the group consisting of n-butyl acrylate, methyl methacrylate, and 2-ethylhexyl acrylate, and more preferably contains at least one selected from the group consisting of n-butyl acrylate, methyl methacrylate, and 2-ethylhexyl acrylate.
[0038] When the specific (meth)acrylic resin particles A contain a structural unit derived from a (meth)acrylic acid alkyl ester monomer, they may contain only one type of structural unit derived from a (meth)acrylic acid alkyl ester monomer, or may contain two or more types of structural units derived from a (meth)acrylic acid alkyl ester monomer.
[0039] When the specific (meth)acrylic resin particles A contain structural units derived from (meth)acrylic acid alkyl ester monomers, the content of the structural units derived from (meth)acrylic acid alkyl ester monomers is not particularly limited, but is, for example, preferably 50% by mass to 98% by mass, more preferably 50% by mass to 85% by mass, and even more preferably 50% by mass to 70% by mass, relative to all structural units of the specific (meth)acrylic resin particles A. Here, the content of structural units derived from (meth)acrylic acid alkyl ester monomers in the specific (meth)acrylic resin particles A being 50% by mass or more relative to all structural units of the specific (meth)acrylic resin particles A means that the structural units derived from (meth)acrylic acid alkyl ester monomers are contained as a main component of the structural units constituting the specific (meth)acrylic resin particles A.
[0040] <Constituent units derived from other monomers> The specific (meth)acrylic resin particles A may contain constituent units derived from monomers (so-called other monomers) that do not fall into any of the following categories: a monomer having a carboxy group, a monomer having a self-crosslinking group, and a (meth)acrylic acid alkyl ester monomer. In the present disclosure, the term "constituent units derived from other monomers" refers to constituent units formed by addition polymerization of other monomers.
[0041] Examples of the structural units derived from other monomers include structural units derived from styrene. When the specific (meth)acrylic resin particles A contain structural units derived from styrene, gloss can be imparted to the coating film formed.
[0042] Furthermore, examples of structural units derived from other monomers include structural units derived from (meth)acrylates having an aromatic ring, such as benzyl (meth)acrylate and phenoxyethyl (meth)acrylate; structural units derived from alkoxyalkyl (meth)acrylates, such as methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate; structural units derived from vinyl cyanide, such as acrylonitrile and methacrylonitrile; and structural units derived from vinyl esters, such as vinyl formate, vinyl acetate, vinyl propionate, and vinyl versatate.
[0043] When the specific (meth)acrylic resin particles A contain a structural unit derived from another monomer, they may contain only one type of structural unit derived from another monomer, or may contain two or more types of structural units derived from another monomer.
[0044] When the specific (meth)acrylic resin particles A contain structural units derived from other monomers, the content of the structural units derived from other monomers can be set appropriately within a range that does not impair the effects of the coating composition of the present disclosure.
[0045] <<Glass Transition Temperature of Specific (Meth)acrylic Resin Particles A>> The glass transition temperature (also referred to as "Tg") of the specific (meth)acrylic resin particles A is 55°C or higher. When the glass transition temperature of the specific (meth)acrylic resin particles A is 55°C or higher, a coating film that exhibits high adhesive strength under high-temperature conditions when bonding magnetic steel sheets together tends to be formed. From this perspective, the glass transition temperature of the specific (meth)acrylic resin particles A is preferably 60°C or higher, more preferably 65°C or higher, and even more preferably 70°C or higher. The upper limit of the glass transition temperature of the specific (meth)acrylic resin particles A is not particularly limited, but is preferably, for example, 80°C or lower. In one embodiment, the glass transition temperature of the specific (meth)acrylic resin particles A may be 55°C to 80°C, 60°C to 80°C, 65°C to 80°C, or 70°C to 80°C.
[0046] The glass transition temperature of the specific (meth)acrylic resin particles A is a value measured by the following method using a differential scanning calorimetry (DSC). An aqueous dispersion of the specific (meth)acrylic resin particles A is applied to a release paper using a 4 mil (101.6 μm) applicator. The applied aqueous dispersion of the specific (meth)acrylic resin particles A is then dried (drying temperature: 105° C., drying time: 10 minutes) to obtain a dried product of the specific (meth)acrylic resin particles A. 10 mg of this dried product is placed in an aluminum sample pan (e.g., Tzero Pan (trade name) manufactured by TA Instrument Co., Ltd.) and sealed with an aluminum lid (e.g., Tzero Hermetic Lid (trade name) manufactured by TA Instrument Co., Ltd.). The glass transition temperature is then measured using a differential scanning calorimetry under the following measurement conditions. In this measurement, the glass transition temperature is the temperature at the intersection of a straight line extending the low-temperature baseline to the high-temperature side of the obtained DSC curve and a tangent drawn at the point where the gradient of the curve in the stepwise change portion of the glass transition is maximum. As the differential scanning calorimeter, for example, a differential scanning calorimeter manufactured by TA Instruments Japan Co., Ltd. (trade name: Discovery DSC 2500) can be used. However, the differential scanning calorimeter is not limited to this.
[0047] - Measurement conditions - Ambient conditions: under air Measurement temperature range: -90°C to 100°C Heating rate: 10°C / min Standard material: empty sample pan
[0048] The glass transition temperature of the specific (meth)acrylic resin particles A can be appropriately adjusted, for example, by using two or more types of monomers that have different glass transition temperatures when made into homopolymers.
[0049] <<Average Primary Particle Diameter of Specific (Meth)acrylic Resin Particles A>> The average primary particle diameter of the specific (meth)acrylic resin particles A is not particularly limited, but from the viewpoint of production stability of the specific (meth)acrylic resin particles A, for example, it is preferably 200 nm to 450 nm, more preferably 230 nm to 450 nm, even more preferably 250 nm to 450 nm, and particularly preferably 280 nm to 400 nm.
[0050] The average primary particle diameter of the specific (meth)acrylic resin particles A can be controlled, for example, by adjusting the amount of surfactant used in producing the specific (meth)acrylic resin particles A. The particle diameter of the specific (meth)acrylic resin particles A tends to be smaller when a larger amount of surfactant is used in producing the specific (meth)acrylic resin particles A, and tends to be larger when a smaller amount of surfactant is used.
[0051] The average primary particle diameter of the specific (meth)acrylic resin particles A refers to the volume-average primary particle diameter. The average primary particle diameter of the specific (meth)acrylic resin particles A is a value measured using a particle size distribution analyzer by the dynamic light scattering method described in "New Experimental Chemistry Lectures 4, Basic Technology 3, Light (II)" edited by the Chemical Society of Japan, pp. 725-741 (published July 20, 1976 by Maruzen Co., Ltd.). The specific method is as follows: 5 mL of the dispersion of the specific (meth)acrylic resin particles A is collected using a Pasteur pipette into a 10 mm square glass cell, which is then set in the particle size distribution analyzer. The attenuation rate (attenuator) is set to x8 (8 times), and the concentration of the dispersion of the specific (meth)acrylic resin particles A is adjusted so that the count rate of the attenuation rate is 150 kCps to 200 kCps. Using a dispersion of specific (meth)acrylic resin particles A with an adjusted concentration, the particle size distribution of the specific (meth)acrylic resin particles A is measured under conditions of a measurement temperature of 25°C and a light scattering angle of 90°. The obtained measurement results are processed by computer to determine the average primary particle diameter of the specific (meth)acrylic resin particles A. Specifically, the particle diameter at an integrated value of 50% (volume basis) in the obtained particle size distribution is defined as the volume-average primary particle diameter. As a particle size distribution measuring device, for example, a "Zetasizer Nano ZS-90" manufactured by Malvern can be suitably used. However, the particle size distribution measuring device is not limited to this.
[0052] <<Content of Specific (Meth)acrylic Resin Particles A>> The content of the specific (meth)acrylic resin particles A in the coating composition of the present disclosure is not particularly limited, but is, for example, preferably 85% by mass to 95% by mass, more preferably 87% by mass to 93% by mass, and even more preferably 89% by mass to 91% by mass, relative to the total solid content in the coating composition.
[0053] In the present disclosure, the "total solid content in the coating composition" refers to the mass of the residue remaining after excluding the solvent from the coating composition. In the present disclosure, the "solvent" refers to water and organic solvents.
[0054] [Method for producing specific (meth)acrylic resin particles A] The method for producing the specific (meth)acrylic resin particles A is not particularly limited as long as it can produce the above-described specific (meth)acrylic resin particles A. The specific (meth)acrylic resin particles A can be produced, for example, by an emulsion polymerization method. Examples of the emulsion polymerization method for producing the specific (meth)acrylic resin particles A include the following methods [1] to [3]. In the following description, the monomer that forms the constituent units of the specific (meth)acrylic resin particles A is also referred to as "monomer component A."
[0055] [1] A method in which a monomer component A, a surfactant, and water are charged into a reactor equipped with a thermometer, a stirrer, a raw material inlet pipe, a reflux condenser, a nitrogen inlet pipe, etc., and the temperature is raised while stirring under a nitrogen stream, and then a polymerization initiator, a reducing agent, etc. are added as appropriate to allow the emulsion polymerization reaction to proceed (the so-called bulk charging method). [2] A method in which at least a surfactant and water are charged into a reactor equipped with a thermometer, a stirrer, a raw material inlet pipe, a reflux condenser, a nitrogen inlet pipe, etc., and the temperature is raised while stirring under a nitrogen stream, and then a monomer component A is added dropwise, and then a polymerization initiator, a reducing agent, etc. are added as appropriate to allow the emulsion polymerization reaction to proceed (the so-called monomer dropping method). [3] In a separate vessel, a monomer component A is pre-emulsified using at least a surfactant and water to prepare a pre-emulsion. A reactor equipped with a thermometer, a stirrer, a raw material inlet pipe, a reflux condenser, a nitrogen inlet pipe, etc., is charged with a portion of the pre-emulsion and water, and the temperature is raised while stirring under a nitrogen stream. After the temperature inside the reactor has stabilized, the remaining pre-emulsion is added dropwise to the reactor while appropriately adding a polymerization initiator, a reducing agent, etc., to allow the emulsion polymerization reaction to proceed (so-called emulsion monomer dropping method). Among these, the emulsion polymerization method for producing the specific (meth)acrylic resin particles A is preferably the emulsion monomer dropping method described above in [3].
[0056] Monomer component A contains a monomer having a carboxy group. Details of the monomer having a carboxy group are as described above. Monomer component A may contain only one type of monomer having a carboxy group, or may contain two or more types of monomers having a carboxy group. The amount of the monomer having a carboxy group used is preferably, for example, in the range of 1 part by mass or more and less than 20 parts by mass per 100 parts by mass of the total of monomer component A.
[0057] The monomer component A includes a monomer having a self-crosslinking group. Details of the monomer having a self-crosslinking group are as described above. The monomer component A may include only one type of monomer having a self-crosslinking group, or may include two or more types. The amount of the monomer having a self-crosslinking group used is preferably, for example, in the range of 0.1 parts by mass or more and 7 parts by mass or less, relative to 100 parts by mass of the total of the monomer component A.
[0058] Monomer component A preferably contains a (meth)acrylic acid alkyl ester monomer. Details of the (meth)acrylic acid alkyl ester monomer are as described above. When monomer component A contains a (meth)acrylic acid alkyl ester monomer, it may contain only one type of (meth)acrylic acid alkyl ester monomer, or may contain two or more types of (meth)acrylic acid alkyl ester monomer. When a (meth)acrylic acid alkyl ester monomer is used, the amount of the (meth)acrylic acid alkyl ester monomer used is preferably, for example, in the range of 50 parts by mass or more and 98 parts by mass or less, relative to 100 parts by mass of the total of monomer component A.
[0059] Monomer component A may contain other monomers such as styrene. Details of other monomers such as styrene are as described above. When styrene is used, the amount of styrene used is preferably, for example, in the range of 10 parts by mass or more and 48 parts by mass or less per 100 parts by mass of the total of monomer component A.
[0060] The surfactant is not particularly limited. The surfactant may be any of anionic surfactants, cationic surfactants, amphoteric surfactants, and nonionic surfactants, or a combination thereof. For example, from the viewpoint of the production stability of the specific (meth)acrylic resin particles A, the surfactant is preferably an anionic surfactant and / or a nonionic surfactant, and more preferably an anionic surfactant and a nonionic surfactant.
[0061] Examples of anionic surfactants include polyoxyalkylene polycyclic phenyl ether sulfates such as polyoxyethylene distyrenated phenyl ether ammonium sulfate, polyoxyalkylene polycyclic phenyl ether sulfates such as polyoxyethylene distyrenated phenyl ether ammonium sulfate, polyoxyalkylene alkyl phenyl ether sulfates such as polyoxyethylene nonylphenyl ether sodium sulfate, polyoxyalkylene alkyl ether sulfates such as polyoxyethylene lauryl ether sodium sulfate, polyoxyalkylene alkyl ether sulfates, polyoxyalkylene alkyl ether sulfates, and alkyl phosphate salts. Examples of nonionic surfactants include polyoxyalkylene alkyl ethers such as polyoxyethylene oleyl ether and polyoxyethylene lauryl ether, and polyoxyalkylene styrenated phenyl ethers such as polyoxyethylene styrenated phenyl ether.
[0062] In the emulsion polymerization method for producing the specific (meth)acrylic resin particles A, only one type of surfactant may be used, or two or more types may be used.
[0063] In the emulsion polymerization method for producing the specific (meth)acrylic resin particles A, the amount of the surfactant used is not particularly limited, but is preferably, for example, 1.5 parts by mass to 10.0 parts by mass per 100 parts by mass of the total of the monomer components A.
[0064] The polymerization initiator is not particularly limited as long as it can be used in ordinary emulsion polymerization. Examples of the polymerization initiator include persulfates, organic peroxides, and azo compounds. Specific examples of persulfates include ammonium persulfate (also known as "ammonium peroxodisulfate"), sodium persulfate, and potassium persulfate. Specific examples of organic peroxides include t-butyl hydroperoxide, benzoyl peroxide, lauroyl peroxide, caproyl peroxide, di-i-propyl peroxydicarbonate, di-2-ethylhexyl peroxydicarbonate, and t-butyl peroxypivalate. Specific examples of azo compounds include 2,2'-azobisisobutyronitrile, 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), 1,1'-azobis(cyclohexane-1-carbonitrile), and 2,2'-azobis(isobutyrate)dimethyl.
[0065] In the emulsion polymerization method for producing the specific (meth)acrylic resin particles A, only one type of polymerization initiator may be used, or two or more types may be used.
[0066] In the emulsion polymerization method for producing the specific (meth)acrylic resin particles A, the amount of the polymerization initiator used is not particularly limited, but is preferably, for example, 0.2 parts by mass to 1.0 parts by mass per 100 parts by mass of the total of the monomer components A.
[0067] A reducing agent may be used together with the polymerization initiator in the emulsion polymerization method for producing the specific (meth)acrylic resin particles A. Specific examples of the reducing agent include sodium metabisulfite, sodium sulfite, sodium hydrogensulfite, sodium pyrosulfite, sodium pyrophosphate, sodium hydroxymethanesulfinate, thioglycolic acid, and sodium thiosulfate.
[0068] In the emulsion polymerization method for producing the specific (meth)acrylic resin particles A, when a reducing agent is used, only one type of reducing agent may be used, or two or more types of reducing agents may be used.
[0069] When a reducing agent is used in the emulsion polymerization method for producing the specific (meth)acrylic resin particles A, the amount of the reducing agent used is not particularly limited, but is preferably, for example, 0.2 parts by mass to 1.0 parts by mass per 100 parts by mass of the total of the monomer components A.
[0070] In the emulsion polymerization method for producing the specific (meth)acrylic resin particles A, the polymerization temperature is, for example, 50° C. to 80° C., and preferably 60° C. to 70° C. The polymerization time is, for example, 5 hours to 9 hours, and preferably 6 hours to 8 hours.
[0071] [Water-soluble (meth)acrylic resin B] The coating composition of the present disclosure contains a water-soluble (meth)acrylic resin B. The coating composition of the present disclosure may contain only one type of water-soluble (meth)acrylic resin B, or may contain two or more types of water-soluble (meth)acrylic resin B. In the coating composition of the present disclosure, the water-soluble (meth)acrylic resin B is present in a dissolved state in a medium containing water.
[0072] In the present disclosure, "water-soluble (meth)acrylic resin" refers to a (meth)acrylic resin having a resin film haze value of 3.0 or less, measured by the following method. The solids concentration of the (meth)acrylic resin is adjusted to 30% by mass using water to prepare a sample solution. The sample solution is applied to one surface of a substrate using a bar coater so that the film thickness after drying is 2 μm, forming a coating film. The formed coating film is then dried at 100°C for 1 minute to obtain a PET-attached resin film. The haze of the obtained PET-attached resin film is measured using a haze meter. The haze value of the resin film is calculated by subtracting the haze value of the PET from the obtained haze value. A polyethylene terephthalate (PET) film is suitable as the substrate. For example, "Lumirror (registered trademark) 125T60" (haze value: 2.63) manufactured by Toray Industries, Inc. can be used as the PET film. However, the substrate is not limited thereto. The haze meter may be, for example, a haze meter (model number: NDH5000 SP) manufactured by Nippon Denshoku Industries Co., Ltd. However, the haze meter is not limited to this.
[0073] <Constituent Units Derived from Monomers Having Self-Crosslinking Groups> The water-soluble (meth)acrylic resin B preferably contains constituent units derived from monomers having self-crosslinking groups. When the water-soluble (meth)acrylic resin B contains constituent units derived from monomers having self-crosslinking groups, the coating film formed tends to exhibit higher adhesive strength under high-temperature conditions when bonding electrical steel sheets together.
[0074] Specific examples of the self-crosslinking group in the water-soluble (meth)acrylic resin B are the same as the specific examples of the self-crosslinking group in the specific (meth)acrylic resin particles A. The self-crosslinking group is preferably at least one selected from the group consisting of an N-methylol group, an N-butyrol group, and a glycidyl group.
[0075] Specific examples of the monomer having a self-crosslinkable group in the water-soluble (meth)acrylic resin B are the same as the specific examples of the monomer having a self-crosslinkable group in the specific (meth)acrylic resin particles A. The monomer having a self-crosslinkable group preferably includes at least one selected from N-methylolacrylamide (NMAM) and hydroxyethylacrylamide (HEAA), and more preferably at least one selected from N-methylolacrylamide (NMAM) and hydroxyethylacrylamide (HEAA).
[0076] When the water-soluble (meth)acrylic resin B contains a structural unit derived from a monomer having a self-crosslinking group, it may contain only one type of structural unit derived from a monomer having a self-crosslinking group, or it may contain two or more types of structural units derived from a monomer having a self-crosslinking group.
[0077] When the water-soluble (meth)acrylic resin B contains a structural unit derived from a monomer having a self-crosslinking group, the content of the structural unit derived from the monomer having a self-crosslinking group is not particularly limited, but is, for example, preferably 0.1% by mass to 10.0% by mass, more preferably 1.0% by mass to 5.0% by mass, and even more preferably 1.5% by mass to 2.0% by mass, relative to all structural units of the water-soluble (meth)acrylic resin B. When the content of the structural unit derived from the monomer having a self-crosslinking group in the water-soluble (meth)acrylic resin B relative to all structural units of the water-soluble (meth)acrylic resin B is within the above range, the formed coating film tends to exhibit higher adhesive strength under the high-temperature conditions used when bonding electrical steel sheets together.
[0078] <Constituent units derived from monomers having hydroxyl groups> The water-soluble (meth)acrylic resin B preferably contains constituent units derived from monomers having hydroxyl groups. In the present disclosure, the term "constituent units derived from monomers having hydroxyl groups" refers to constituent units formed by addition polymerization of monomers having hydroxyl groups. In the present disclosure, the hydroxyl groups constituting part of the self-crosslinking groups are not included in the hydroxyl groups in the monomers having hydroxyl groups.
[0079] Examples of the monomer having a hydroxyl group include a monomer having at least one hydroxyl group and an ethylenically unsaturated group in one molecule. The ethylenically unsaturated group is not particularly limited, and examples thereof include a vinyl group, an allyl group, a vinylphenyl group, a (meth)acrylamide group, and a (meth)acryloyl group. The ethylenically unsaturated group is preferably a (meth)acryloyl group.
[0080] Specific examples of the monomer having a hydroxyl group include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, 3-methyl-3-hydroxybutyl (meth)acrylate, 1,1-dimethyl-3-hydroxybutyl (meth)acrylate, 1,3-dimethyl-3-hydroxybutyl (meth)acrylate, 2,2,4-trimethyl-3-hydroxypentyl (meth)acrylate, 2-ethyl-3-hydroxyhexyl (meth)acrylate, glycerin mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, polyethylene glycol mono(meth)acrylate, and poly(ethylene glycol-propylene glycol) mono(meth)acrylate. The hydroxyl group-containing monomer preferably includes a hydroxyalkyl(meth)acrylate, more preferably a hydroxyalkyl(meth)acrylate. As the hydroxyalkyl(meth)acrylate, a hydroxyalkyl(meth)acrylate having a hydroxyalkyl group having 2 to 4 carbon atoms is preferred, 2-hydroxyethyl(meth)acrylate is more preferred, and 2-hydroxyethyl methacrylate is even more preferred.
[0081] When the water-soluble (meth)acrylic resin B contains a structural unit derived from a monomer having a hydroxyl group, it may contain only one type of structural unit derived from a monomer having a hydroxyl group, or it may contain two or more types of structural units derived from a monomer having a hydroxyl group.
[0082] When the water-soluble (meth)acrylic resin B contains structural units derived from monomers having a hydroxyl group, the content of the structural units derived from monomers having a hydroxyl group is not particularly limited, but is preferably 5% to 30% by mass, more preferably 10% to 25% by mass, and even more preferably 15% to 25% by mass, relative to all structural units of the water-soluble (meth)acrylic resin B. When the content of structural units derived from monomers having a hydroxyl group in the water-soluble (meth)acrylic resin B is 5% by mass or more relative to all structural units of the water-soluble (meth)acrylic resin B, the adhesive performance of the formed coating film tends to be further improved. When the content of structural units derived from monomers having a hydroxyl group in the water-soluble (meth)acrylic resin B is 30% by mass or less relative to all structural units of the water-soluble (meth)acrylic resin B, the production stability of the water-soluble (meth)acrylic resin B tends to be more excellent.
[0083] <Structural Units Derived from (Meth)acrylic Acid Alkyl Ester Monomers> The water-soluble (meth)acrylic resin B preferably contains structural units derived from (meth)acrylic acid alkyl ester monomers. Note that the "(meth)acrylic acid alkyl ester monomer" in the water-soluble (meth)acrylic resin B does not include monomers corresponding to monomers having a self-crosslinkable group or monomers corresponding to monomers having a hydroxyl group.
[0084] The type of (meth)acrylic acid alkyl ester monomer is not particularly limited. The (meth)acrylic acid alkyl ester monomer may be an acrylic acid alkyl ester monomer or a methacrylic acid alkyl ester monomer. The alkyl group contained in the (meth)acrylic acid alkyl ester monomer may be unsubstituted or may have a substituent (excluding a carboxy group, a self-crosslinkable group, and a hydroxyl group), but is preferably unsubstituted. The alkyl group contained in the (meth)acrylic acid alkyl ester monomer may be linear, branched, or cyclic. The number of carbon atoms in the alkyl group contained in the (meth)acrylic acid alkyl ester monomer is, for example, preferably 1 to 12, more preferably 1 to 8, and even more preferably 1 to 4.
[0085] Specific examples of the (meth)acrylic acid alkyl ester monomer in the water-soluble (meth)acrylic resin B are the same as the specific examples of the (meth)acrylic acid alkyl ester monomer in the specific (meth)acrylic resin particles (A). From the viewpoint of water solubility, the (meth)acrylic acid alkyl ester monomer preferably contains at least one selected from the group consisting of n-butyl acrylate, methyl methacrylate, and ethyl acrylate, more preferably contains at least one selected from methyl methacrylate and ethyl acrylate, and even more preferably contains methyl methacrylate.
[0086] When the water-soluble (meth)acrylic resin B contains a structural unit derived from a (meth)acrylic acid alkyl ester monomer, it may contain only one type of structural unit derived from a (meth)acrylic acid alkyl ester monomer, or it may contain two or more types of structural units derived from a (meth)acrylic acid alkyl ester monomer.
[0087] When the water-soluble (meth)acrylic resin B contains a structural unit derived from a (meth)acrylic acid alkyl ester monomer, the content of the structural unit derived from a (meth)acrylic acid alkyl ester monomer in the water-soluble (meth)acrylic resin B is not particularly limited, but is, for example, preferably 40% by mass to 90% by mass, more preferably 40% by mass to 80% by mass, and even more preferably 40% by mass to 70% by mass, relative to all structural units of the water-soluble (meth)acrylic resin B.
[0088] <Structural Units Derived from Other Monomers> The water-soluble (meth)acrylic resin B may contain structural units derived from monomers (so-called other monomers) that do not fall into any of the categories of monomers having a self-crosslinkable group, monomers having a hydroxyl group, and alkyl (meth)acrylate monomers.
[0089] Examples of structural units derived from other monomers include structural units derived from (meth)acrylates having an aromatic ring, such as benzyl (meth)acrylate and phenoxyethyl (meth)acrylate; structural units derived from alkoxyalkyl (meth)acrylates, such as methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate; structural units derived from vinyl cyanide, such as acrylonitrile and methacrylonitrile; and structural units derived from vinyl esters, such as vinyl formate, vinyl acetate, vinyl propionate, and vinyl versatate.
[0090] When the water-soluble (meth)acrylic resin B contains a structural unit derived from another monomer, it may contain only one type of structural unit derived from another monomer, or may contain two or more types of structural units derived from another monomer.
[0091] When the water-soluble (meth)acrylic resin B contains a structural unit derived from another monomer, the content of the structural unit derived from the other monomer can be set appropriately within a range that does not impair the effects of the coating composition of the present disclosure.
[0092] <<Glass Transition Temperature of Water-Soluble (Meth)acrylic Resin B>> The glass transition temperature of the water-soluble (meth)acrylic resin B is not particularly limited, but is, for example, preferably 100°C or lower, more preferably 90°C or lower, and even more preferably 80°C or lower. When the glass transition temperature of the water-soluble (meth)acrylic resin B is 100°C or lower, the water-soluble (meth)acrylic resin B tends to have excellent film-forming properties. The lower limit of the glass transition temperature of the water-soluble (meth)acrylic resin B is, for example, preferably −70°C or higher.
[0093] The glass transition temperature of the water-soluble (meth)acrylic resin B can be determined by the same method as that for determining the glass transition temperature of the specific (meth)acrylic resin particles A described above.
[0094] The glass transition temperature of the water-soluble (meth)acrylic resin B can be appropriately adjusted, for example, by using two or more kinds of monomers which, when made into homopolymers, have different glass transition temperatures.
[0095] <<Weight-Average Molecular Weight of Water-Soluble (Meth)acrylic Resin B>> The weight-average molecular weight (hereinafter also referred to as "Mw") of the water-soluble (meth)acrylic resin B is not particularly limited, but is, for example, preferably 1,000 to 100,000, more preferably 5,000 to 50,000, and even more preferably 8,000 to 30,000. When the weight-average molecular weight of the water-soluble (meth)acrylic resin B is 1,000 or more, the adhesive performance of the formed coating film tends to be better. When the weight-average molecular weight of the water-soluble (meth)acrylic resin B is 100,000 or less, the production stability of the water-soluble (meth)acrylic resin B and the coatability of the coating composition tend to be better.
[0096] The weight-average molecular weight of the water-soluble (meth)acrylic resin B is a value measured by the following method. Specifically, it is measured according to the following steps (1) to (3). (1) A solution of the water-soluble (meth)acrylic resin B is applied to a release paper and dried at 100°C for 1 minute to obtain a film of the water-soluble (meth)acrylic resin B. (2) The film of the water-soluble (meth)acrylic resin B obtained in step (1) above and tetrahydrofuran are used to obtain a sample solution having a solids concentration of 0.2% by mass. Note that the "solids concentration" here refers to the mass proportion of the water-soluble (meth)acrylic resin B in the sample solution. (3) The weight-average molecular weight of the water-soluble (meth)acrylic resin B is measured as a standard polystyrene equivalent value using gel permeation chromatography (GPC) under the following conditions.
[0097] Conditions: Measurement device: High-speed GPC [Model: HLC-8220 GPC, manufactured by Tosoh Corporation] Detector: Differential refractometer (RI) [Installed in HLC-8220, manufactured by Tosoh Corporation] Column: TSKgel GMH XL Four columns (manufactured by Tosoh Corporation) were used. Column temperature: 40°C. Eluent: tetrahydrofuran. Sample solution injection volume: 100 μL. Flow rate: 0.8 mL / min.
[0098] The weight average molecular weight of the water-soluble (meth)acrylic resin B can be adjusted to a desired value by adjusting the polymerization temperature, polymerization time, the type and amount of polymerization initiator used, the type and amount of chain transfer agent used, and the like.
[0099] <<Content of Water-Soluble (Meth)acrylic Resin B>> The content of water-soluble (meth)acrylic resin B in the coating composition of the present disclosure is not particularly limited, as long as the ratio of the mass content of the specific (meth)acrylic resin particles A to the mass content of the water-soluble (meth)acrylic resin B [mass content of specific (meth)acrylic resin particles A / mass content of water-soluble (meth)acrylic resin B] is 95 / 5 to 85 / 15. When the coating composition of the present disclosure has a mass content ratio of the specific (meth)acrylic resin particles A to the mass content of the water-soluble (meth)acrylic resin B of 95 / 5 to 85 / 15, it can achieve both excellent coating on the surface of the magnetic steel sheet and the formation of a coating film that exhibits high adhesive strength under high-temperature conditions when bonding magnetic steel sheets together. For example, from the viewpoint of forming a coating film that exhibits higher adhesive strength, the ratio of the mass content of the specific (meth)acrylic resin particles A to the mass content of the water-soluble (meth)acrylic resin B is preferably 95 / 5 to 90 / 10.
[0100] [Method for Producing Water-Soluble (Meth)acrylic Resin B] The method for producing the water-soluble (meth)acrylic resin B is not particularly limited as long as it can produce the water-soluble (meth)acrylic resin B described above. The water-soluble (meth)acrylic resin B can be produced, for example, by the following method. First, a dispersion containing (meth)acrylic resin particles having a carboxy group as a dispersoid is prepared by emulsion polymerization using a monomer component containing at least a monomer having a carboxy group. Next, a base is added to the prepared dispersion to neutralize the carboxy groups of the (meth)acrylic resin particles. In this manner, the water-soluble (meth)acrylic resin B is obtained. It is believed that neutralization of the carboxy groups of the (meth)acrylic resin particles promotes dissociation of the carboxy groups, increasing the acidity, which breaks down the micelles and makes the (meth)acrylic resin water-soluble.
[0101] Examples of emulsion polymerization methods for producing the water-soluble (meth)acrylic resin B include the following methods [1] to [3]. In the following description, the monomer that forms the structural unit of the water-soluble (meth)acrylic resin B is also referred to as "monomer component B."
[0102] [1] A method in which a monomer component B, a surfactant, and water are charged into a reactor equipped with a thermometer, a stirrer, a raw material inlet pipe, a reflux condenser, a nitrogen inlet pipe, etc., and the temperature is raised while stirring under a nitrogen stream, and then a polymerization initiator, a reducing agent, a chain transfer agent, etc. are added as appropriate to allow the emulsion polymerization reaction to proceed (the so-called bulk charging method). [2] A method in which at least a surfactant and water are charged into a reactor equipped with a thermometer, a stirrer, a raw material inlet pipe, a reflux condenser, a nitrogen inlet pipe, etc., and the temperature is raised while stirring under a nitrogen stream, and then a monomer component B is added dropwise, and then a polymerization initiator, a reducing agent, a chain transfer agent, etc. are added as appropriate to allow the emulsion polymerization reaction to proceed (the so-called monomer dropping method). [3] In a separate vessel, a monomer component B is emulsified in advance using at least a surfactant and water to prepare a pre-emulsion. A reactor equipped with a thermometer, a stirrer, a raw material inlet pipe, a reflux condenser, a nitrogen inlet pipe, etc. is charged with a portion of the pre-emulsion and water, and the temperature is raised while stirring under a nitrogen stream. After the temperature in the reactor has stabilized, the remaining pre-emulsion is added dropwise to the reactor while appropriately adding a polymerization initiator, a reducing agent, a chain transfer agent, etc., to allow the emulsion polymerization reaction to proceed (the so-called emulsion monomer dropping method). Among these, the emulsion polymerization method for producing the water-soluble (meth)acrylic resin B is preferably the emulsion monomer dropping method described above in [3].
[0103] Monomer component B includes a monomer having a carboxy group. Examples of the monomer having a carboxy group include a monomer having at least one carboxy group and an ethylenically unsaturated group in one molecule. The ethylenically unsaturated group is not particularly limited, and examples include a vinyl group, an allyl group, a vinylphenyl group, a (meth)acrylamide group, and a (meth)acryloyl group. The ethylenically unsaturated group is preferably a (meth)acryloyl group. Specific examples of the monomer having a carboxy group contained in monomer component B are the same as the specific examples of the monomer having a carboxy group in the specific (meth)acrylic resin particles A. The monomer having a carboxy group is preferably a (meth)acrylic monomer having a carboxy group, more preferably (meth)acrylic acid, and even more preferably acrylic acid. Monomer component B may include only one type of monomer having a carboxy group, or may include two or more types. The amount of the carboxyl group-containing monomer used is preferably, for example, in the range of 10 parts by mass or more and 30 parts by mass or less per 100 parts by mass of the total of the monomer component B.
[0104] The monomer component B preferably contains a monomer having a self-crosslinking group. Details of the monomer having a self-crosslinking group are as described above. When the monomer component B contains a monomer having a self-crosslinking group, it may contain only one type of monomer having a self-crosslinking group, or may contain two or more types of monomers having a self-crosslinking group. When a monomer having a self-crosslinking group is used, the amount of the monomer having a self-crosslinking group used is preferably, for example, in the range of 1 part by mass or more and 5 parts by mass or less, relative to a total of 100 parts by mass of the monomer component B.
[0105] It is preferable that the monomer component B contains a monomer having a hydroxyl group. Details of the monomer having a hydroxyl group are as described above. When the monomer component B contains a monomer having a hydroxyl group, it may contain only one type of monomer having a hydroxyl group, or may contain two or more types of monomers having a hydroxyl group. When a monomer having a hydroxyl group is used, the amount of the monomer having a hydroxyl group used is preferably, for example, in the range of 10 parts by mass or more and 30 parts by mass or less, relative to 100 parts by mass of the total of the monomer component B.
[0106] Monomer component B preferably contains a (meth)acrylic acid alkyl ester monomer. Details of the (meth)acrylic acid alkyl ester monomer are as described above. When monomer component B contains a (meth)acrylic acid alkyl ester monomer, it may contain only one type of (meth)acrylic acid alkyl ester monomer, or may contain two or more types of (meth)acrylic acid alkyl ester monomer. When a (meth)acrylic acid alkyl ester monomer is used, the amount of the (meth)acrylic acid alkyl ester monomer used is preferably, for example, in the range of 40 parts by mass or more and 80 parts by mass or less, relative to 100 parts by mass of the total of monomer component B.
[0107] The type of surfactant is not particularly limited. The surfactant may be any of anionic surfactants, cationic surfactants, amphoteric surfactants, or nonionic surfactants, or a combination thereof. For example, from the viewpoint of production stability of the water-soluble (meth)acrylic resin B, the surfactant is preferably an anionic surfactant and / or a nonionic surfactant, and more preferably an anionic surfactant. Specific examples of the anionic surfactant are the same as the specific examples of the anionic surfactant in the emulsion polymerization method for producing the specific (meth)acrylic resin particles A. Specific examples of the nonionic surfactant are the same as the specific examples of the nonionic surfactant in the emulsion polymerization method for producing the specific (meth)acrylic resin particles A.
[0108] In the emulsion polymerization method for producing the water-soluble (meth)acrylic resin B, only one surfactant may be used, or two or more surfactants may be used.
[0109] In the emulsion polymerization method for producing the water-soluble (meth)acrylic resin B, the amount of the surfactant used is not particularly limited, but is preferably, for example, 0.5 parts by mass to 5.0 parts by mass per 100 parts by mass of the total of the monomer components B.
[0110] The polymerization initiator is not particularly limited as long as it can be used in normal emulsion polymerization. Examples of the polymerization initiator include persulfates, organic peroxides, and azo compounds. Specific examples of the persulfates, organic peroxides, and azo compounds are the same as the specific examples of the persulfates, organic peroxides, and azo compounds in the emulsion polymerization method for producing the specific (meth)acrylic resin particles A.
[0111] In the emulsion polymerization method for producing the water-soluble (meth)acrylic resin B, only one type of polymerization initiator may be used, or two or more types may be used.
[0112] In the emulsion polymerization method for producing the water-soluble (meth)acrylic resin B, the amount of the polymerization initiator used is not particularly limited, but is preferably, for example, 0.5 parts by mass to 3.0 parts by mass per 100 parts by mass of the total of the monomer components B.
[0113] A reducing agent may be used together with the polymerization initiator in the emulsion polymerization method for producing the water-soluble (meth)acrylic resin B. Specific examples of the reducing agent are the same as those of the reducing agent in the emulsion polymerization method for producing the specific (meth)acrylic resin particles A.
[0114] In the emulsion polymerization method for producing the water-soluble (meth)acrylic resin B, when a reducing agent is used, only one reducing agent may be used, or two or more reducing agents may be used.
[0115] When a reducing agent is used in the emulsion polymerization method for producing the water-soluble (meth)acrylic resin B, the amount of the reducing agent used is not particularly limited, but is preferably, for example, 0.1 parts by mass to 1.0 parts by mass per 100 parts by mass of the total of the monomer components B.
[0116] The type of chain transfer agent is not particularly limited. Specific examples of the chain transfer agent include cyanoacetic acid, alkyl ester compounds of cyanoacetic acid having 1 to 8 carbon atoms, bromoacetic acid, alkyl ester compounds of bromoacetic acid having 1 to 8 carbon atoms, aromatic compounds represented by α-methylstyrene, anthracene, phenanthrene, fluorene, and 9-phenylfluorene, aromatic nitro compounds represented by p-nitroaniline, nitrobenzene, dinitrobenzene, p-nitrobenzoic acid, p-nitrophenol, and p-nitrotoluene, benzoquinone derivatives represented by benzoquinone and 2,3,5,6-tetramethyl-p-benzoquinone, borane derivatives represented by tributylborane, carbon tetrabromide, carbon tetrachloride, 1,1, Examples of the halogenated hydrocarbon compounds include 2,2-tetrabromoethane, tribromoethylene, trichloroethylene, bromotrichloromethane, tribromomethane, and 3-chloro-1-propene; aldehyde compounds include chloral and furaldehyde; alkyl mercaptan compounds having 1 to 18 carbon atoms; aromatic mercaptan compounds include thiophenol and toluene mercaptan; mercaptoacetic acid; alkyl ester compounds of mercaptoacetic acid having 1 to 10 carbon atoms; hydroxyalkyl mercaptan compounds having 1 to 12 carbon atoms (for example, 2-mercaptoethanol); and terpene compounds include pinene and terpinolene.
[0117] In the emulsion polymerization method for producing the water-soluble (meth)acrylic resin B, when a chain transfer agent is used, only one type of chain transfer agent may be used, or two or more types of chain transfer agents may be used.
[0118] When a chain transfer agent is used in the emulsion polymerization method for producing the water-soluble (meth)acrylic resin B, the amount of the chain transfer agent used is not particularly limited, but is preferably, for example, 1 part by mass to 3 parts by mass per 100 parts by mass of the total of the monomer components B.
[0119] In the emulsion polymerization method for producing the water-soluble (meth)acrylic resin B, the polymerization temperature is, for example, 58° C. to 62° C., and preferably 59° C. to 61° C. The polymerization time is, for example, 3 hours to 6 hours, and preferably 4 hours to 5 hours.
[0120] According to the emulsion polymerization method, a dispersion containing (meth)acrylic resin particles as dispersoids is obtained. A base is added to the obtained dispersion to neutralize the carboxy groups of the (meth)acrylic resin particles, thereby producing a water-soluble (meth)acrylic resin B. Specific examples of the base include aqueous ammonia (aqueous ammonium hydroxide solution) and aqueous sodium hydroxide solution. As the base, for example, aqueous ammonia is preferred from the viewpoint of the adhesive properties of the coating film.
[0121] [Water] The coating composition of the present disclosure contains water. The type of water is not particularly limited. As the water, for example, distilled water, deionized water (also called "ion-exchanged water"), and pure water are preferred from the viewpoint of having few impurities.
[0122] The water content in the coating composition of the present disclosure is not particularly limited, but is, for example, preferably 35% by mass to 50% by mass, and more preferably 40% by mass to 45% by mass, relative to the total mass of the coating composition.
[0123] [Other Components] The coating composition of the present disclosure may contain components (so-called other components) other than the components described above, as needed, within the range that does not impair the effects of the coating composition.
[0124] Examples of other components include aqueous media other than water. Examples of aqueous media other than water include water-miscible organic solvents. Examples of water-miscible organic solvents include monohydric alcohol compounds such as methanol and ethanol; polyhydric alcohol compounds such as glycerin, ethylene glycol, and propylene glycol; and glycol derivatives such as ethylene glycol monoethyl ether and propylene glycol monobutyl ether. Examples of other components include various additives such as preservatives, wetting agents, and antifoaming agents.
[0125] [Gel Fraction of Coating Composition] The coating composition of the present disclosure preferably has a gel fraction at a temperature higher than the temperature at which crosslinking by the self-crosslinking groups contained in the specific (meth)acrylic resin particles A proceeds, which is greater than the gel fraction at a temperature lower than the temperature at which crosslinking by the self-crosslinking groups contained in the specific (meth)acrylic resin particles A proceeds. When the gel fraction of the coating composition of the present disclosure satisfies the above-mentioned requirements, the coating composition of the present disclosure tends to achieve a good balance between excellent application to the surfaces of magnetic steel sheets and the formation of a coating film that exhibits high adhesive strength under high-temperature conditions when bonding magnetic steel sheets together.
[0126] The gel fraction of the coating composition of the present disclosure is the proportion of solvent-insoluble matter measured using ethyl acetate as an extraction solvent. Specifically, the gel fraction of the coating composition of the present disclosure can be determined according to the following procedures [1] to
[17] .
[0127] [1] Ammonia water is added to the coating composition of the present disclosure to adjust the pH to 8.5 (liquid temperature 25°C). The resulting solution is then applied to a 100 μm-thick polyethylene terephthalate (PET) release film to form a coating film. The formed coating film is then dried at 105°C for 2 minutes to obtain a resin film with a release film. [2] The resulting resin film with a release film is cut into a size of 75 mm x 75 mm. The weight of the cut resin film with a release film is approximately 0.2 g. [3] A 250-mesh stainless steel wire mesh (wire diameter: 0.03 mm, mesh size: 72 μm) is prepared, and this wire mesh is cut into a size of 100 mm x 100 mm. Note that loose ends of the wire mesh are removed in advance to prevent measurement errors. [4] The cut wire mesh is degreased with ethyl acetate and then dried. The dried wire mesh is stored in a desiccator. [5] The mass of the wire mesh is accurately measured. The measured mass of the wire mesh is designated as A (unit: g). [6] The resin film with release film described above in [2], cut to a size of 75 mm x 75 mm, is attached to the center of the wire mesh, and then the release film is peeled off from the resin film to obtain a wire mesh with a resin film. The resin film is attached to the wire mesh so that the resin film is positioned within the plane of the wire mesh after folding in the steps [7] to [9] described below. [7] The wire mesh with a resin film is folded in half with the resin film facing inward. Specifically, the wire mesh with a resin film is folded so that the rear edge of the wire mesh with a resin film overlaps the front edge. [8] The front third of the half-folded wire mesh with a resin film (the side where the two edges overlap) is folded toward the rear, and then the rear third is folded toward the front. At this point, the resin-coated wire mesh has been folded lengthwise to one-sixth of its original size (100 mm), and is not folded widthwise. [9] The left one-third of the longitudinal length of the resin-coated wire mesh folded in [8] above is folded to the right, and then the right one-third is folded to the left. This is designated Sample X1. Sample X1 has been folded lengthwise to one-sixth of its original size (100 mm), and is folded widthwise to one-third.
[10] The mass of Sample X1 is accurately measured using a precision balance. This mass is designated B (unit: g).
[11] Staple the folds of sample X1 to prevent them from unfolding. This is sample X2. Two samples of sample X2 are prepared per sample.
[12] Accurately measure the mass of sample X2 using a precision balance. This mass is designated C (unit: g).
[13] Place sample X2 in a glass bottle containing 80 g of ethyl acetate and close the lid.
[14] Leave the glass bottle containing sample X2 in an environment with an ambient temperature of 23°C and 50% RH for three days.
[15] Remove sample X2 from the glass bottle and wash it with a small amount of ethyl acetate.
[16] Dry sample X2 at a drying temperature of 100°C for 24 hours. Accurately measure the mass of sample X2 after drying using a precision balance. This mass is designated D (unit: g).
[17] Calculate the gel fraction using the following formula, and take the arithmetic average of the obtained values. Gel fraction [mass%]=(D−(A+(C−B))) / (B−A)×100.
[0128] [Uses of Coating Composition] The coating composition of the present disclosure is used to coat the surface of an electrical steel sheet used in the production of a laminated steel sheet. The coating composition of the present disclosure can form a coating film that exhibits high adhesive strength under the high-temperature conditions used when bonding electrical steel sheets together, and has excellent coatability, so a specific use thereof includes fixing electrical steel sheets together when producing a laminated steel sheet. The coating composition of the present disclosure is suitable, for example, for forming an adhesive coating on an adhesive-coated electrical steel sheet used in the production of a laminated steel sheet.
[0129] [Electromagnetic steel sheet] The electromagnetic steel sheet is a steel sheet on which an adhesive coating is formed, and is not particularly limited. The electromagnetic steel sheet may be a non-oriented electromagnetic steel sheet or a grain-oriented electromagnetic steel sheet. Specifically, the electromagnetic steel sheet may be, for example, a non-oriented electromagnetic steel sheet according to JIS C 2552:2014, a grain-oriented electromagnetic steel sheet according to JIS C 2553:2019, or a non-oriented thin-film electromagnetic steel sheet or grain-oriented thin-film electromagnetic steel sheet according to JIS C 2558:2015.
[0130] [Method for Producing Coating Composition] The method for producing the coating composition of the present disclosure is not particularly limited. The coating composition of the present disclosure can be produced, for example, by mixing a dispersion of specific (meth)acrylic resin particles A and an aqueous solution of water-soluble (meth)acrylic resin B so that the mass ratio [A / B] of the specific (meth)acrylic resin particles A to the water-soluble (meth)acrylic resin B is 95 / 5 to 85 / 15.
[0131] The mixing method is not particularly limited. For example, mixing by stirring can be used. A general stirring tool or stirring device can be used for stirring. The stirring temperature is not particularly limited, but is preferably, for example, 20°C to 30°C.
[0132] The coating composition of the present disclosure will be described in more detail below with reference to examples. The present disclosure is not limited to the following examples as long as it does not deviate from the gist of the disclosure.
[0133] [Production of Coating Composition] [Example 1] 1. Production of (meth)acrylic resin particles A A monomer mixture was prepared by mixing 54.4 parts by mass of n-butyl acrylate [n-BA; acrylic acid alkyl ester monomer], 169.5 parts by mass of methyl methacrylate [MMA; methacrylic acid alkyl ester monomer], 128.4 parts by mass of styrene [St; other monomer], 40 parts by mass of methacrylic acid [MAA; monomer having a carboxy group], and 7.8 parts by mass of hydroxyethyl acrylamide [HEAA; monomer having a self-crosslinkable group] in a stainless steel container. Next, 172.0 parts by mass of deionized water, 2.7 parts by mass of the nonionic surfactant Noigen (registered trademark) EA-197D (manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.), 4.1 parts by mass of Emulgen (registered trademark) A-60 (manufactured by Kao Corporation), and 2.7 parts by mass of the anionic surfactant Neopelex (registered trademark) G-65 (manufactured by Kao Corporation) were placed in a separate stainless steel container and stirred to dissolve, thereby preparing an aqueous surfactant solution. Next, the monomer mixture prepared above was gradually added to the aqueous surfactant solution while stirring with a stirrer to emulsify, thereby preparing a pre-emulsion. This prepared pre-emulsion was used for polymerization. The polymerization was carried out in a thermostatic chamber equipped with a 7 L (liter; the same applies hereinafter) flask, a reflux condenser, a stirrer, a nitrogen gas inlet pipe, a pre-emulsion dropping pump (trade name: Hi-Cera Pump V-10, manufactured by Iwaki Corporation), and a polymerization initiator adding device (trade name: Metering Pump MP-2000, manufactured by Tokyo Rikakikai Co., Ltd.). Specifically, the polymerization was carried out as follows. 162.4 parts by mass of deionized water was placed in the flask, and then a portion (17.5 parts by mass) of the pre-emulsion prepared above was added. Nitrogen gas was blown into the flask at a flow rate of 300 ml / min, and the internal temperature of the flask was raised to a desired reaction temperature (standard conditions: 62°C) while stirring at a desired rotation speed (standard conditions: 240 rpm (revolutions per minute; the same applies hereinafter)). After the internal temperature stabilized, 2.3 parts by mass of a 24% by mass aqueous solution of ammonium peroxodisulfate (polymerization initiator) and 2.3 parts by mass of a 20% by mass aqueous solution of sodium hydrogen sulfite (reducing agent) were added, and the flow rate of nitrogen gas was adjusted to 50 ml / min.After confirming the temperature increase in the flask, the remaining pre-emulsion (564 parts by mass) was added dropwise over 270 minutes, and 63.4 parts by mass of a 2.4% by mass aqueous solution of ammonium peroxodisulfate (polymerization initiator) and 63.4 parts by mass of a 2.0% by mass aqueous solution of sodium hydrogen sulfite (reducing agent) were added dropwise over 360 minutes. Thirty minutes after the completion of the dropwise addition of the aqueous solution of ammonium peroxodisulfate and sodium hydrogen sulfite, 6.4 parts by mass of a 6.9% by mass aqueous solution of t-butyl hydroperoxide (polymerization initiator) and 6.4 parts by mass of a 4.4% by mass aqueous solution of sodium hydroxymethanesulfinate (reducing agent) were added dropwise over 30 minutes. The polymerization reaction was terminated 150 minutes after the completion of the dropwise addition of the pre-emulsion by cooling to 30°C. To the emulsion polymer obtained by the polymerization reaction, 1.3 parts by mass of a preservative (trade name: Topside 350, manufactured by Permakem Asia Co., Ltd.) and 1.3 parts by mass of a wetting agent (trade name: Surfynol (registered trademark) 440, manufactured by Nissin Chemical Industry Co., Ltd.) were added to obtain an aqueous dispersion of (meth)acrylic resin particles A.
[0134] 2. Preparation of Water-Soluble (Meth)acrylic Resin B 126.2 parts by mass of methyl methacrylate (MMA; methacrylic acid alkyl ester monomer), 48.0 parts by mass of ethyl acrylate (EA; acrylic acid alkyl ester monomer), 60.0 parts by mass of acrylic acid (AA; monomer having a carboxy group), 60.0 parts by mass of 2-hydroxyethyl methacrylate (2HEMA; monomer having a hydroxyl group), and 5.8 parts by mass of hydroxyethyl acrylamide (HEAA; monomer having a self-crosslinking group) were mixed in a stainless steel container to prepare a monomer mixture. Next, 121.0 parts by mass of deionized water and 4.5 parts by mass of the anionic surfactant Latemul (registered trademark) E-118B (manufactured by Kao Corporation) were added to another stainless steel container, and the mixture was stirred to dissolve, preparing an aqueous surfactant solution. Next, the monomer mixture prepared above was gradually added to the aqueous surfactant solution while stirring with a stirrer to emulsify, thereby preparing a pre-emulsion. This prepared pre-emulsion was used for polymerization. The polymerization was carried out in a thermostatic chamber equipped with a 7 L flask equipped with a reflux condenser, a stirrer, a nitrogen gas inlet pipe, a pre-emulsion drip pump (trade name: Hi-Cera Pump V-10, manufactured by Iwaki Corporation), and a polymerization initiator addition device (trade name: Metering Pump MP-2000, manufactured by Tokyo Rikakikai Co., Ltd.). Specifically, the polymerization was carried out as follows. 415 parts by mass of deionized water and 7.0 parts by mass of an anionic surfactant, Latemul (registered trademark) E-118B (manufactured by Kao Corporation), were placed in a flask, and then a portion (8.5 parts by mass) of the pre-emulsion prepared above was added. Nitrogen gas was blown into the flask at a flow rate of 300 ml / min, and while stirring at a desired rotation speed (standard conditions: 150 rpm), the internal temperature of the flask was raised to a desired reaction temperature (standard conditions: 60°C), and then 1.0 part by mass of a 69.0% by mass aqueous solution of t-butyl hydroperoxide (polymerization initiator) and 2.5 parts by mass of a 10.0% by mass aqueous solution of sodium hydroxymethanesulfinate (reducing agent) were added. After the internal temperature stabilized, the flow rate of the nitrogen gas was adjusted to 50 ml / min.After the adjustment, the remaining pre-emulsion (456.6 parts by mass) was added dropwise over 180 minutes, and 24.5 parts by mass of a 6.9% by mass aqueous solution of t-butyl hydroperoxide (polymerization initiator), 24.5 parts by mass of a 1.2% by mass aqueous solution of sodium hydroxymethanesulfinate (reducing agent), and 39.6 parts by mass of 14.7% by mass 2-mercaptoethanol (chain transfer agent) were added dropwise over 180 minutes to obtain an aqueous dispersion of (meth)acrylic resin particles. 58 parts by mass of 25.0% by mass aqueous ammonia (basic aqueous solution) was added to the obtained aqueous dispersion of (meth)acrylic resin particles to solubilize the (meth)acrylic resin particles, thereby obtaining an aqueous solution of water-soluble (meth)acrylic resin B.
[0135] 3. Preparation of Coating Composition 300.0 parts by mass (137.1 parts by mass as solids) of an aqueous dispersion of (meth)acrylic resin particles A and 48.1 parts by mass (15.2 parts by mass as solids) of an aqueous solution of water-soluble (meth)acrylic resin B were mixed, and then an appropriate amount of deionized water was added to obtain a coating composition with a solids concentration of 43.5% by mass. The "solids concentration" here refers to the total mass proportion of the (meth)acrylic resin particles A and the water-soluble (meth)acrylic resin B in the coating composition. The same applies to the coating compositions prepared below.
[0136] Examples 2 to 10 The same operation as in Example 1 was carried out, except that the monomer compositions of the (meth)acrylic resin particles A and the water-soluble (meth)acrylic resin B were set to the monomer compositions shown in Table 1, and the mass ratio [A / B] of the (meth)acrylic resin particles A to the water-soluble (meth)acrylic resin B was set to the mass ratio shown in Table 1, to obtain coating compositions with a solid content concentration of 43.5 mass%.
[0137] Examples 11 to 21 The same operation as in Example 1 was carried out to obtain coating compositions with a solid content concentration of 43.5 mass %, except that the monomer compositions of the (meth)acrylic resin particles A and the water-soluble (meth)acrylic resin B were set to the monomer compositions shown in Table 2, and the mass ratio [A / B] of the (meth)acrylic resin particles A to the water-soluble (meth)acrylic resin B was set to the mass ratio shown in Table 2.
[0138] Comparative Examples 1 to 8 The same operation as in Example 1 was carried out, except that the monomer compositions of the (meth)acrylic resin particles A and the water-soluble (meth)acrylic resin B were set to the monomer compositions shown in Table 3, and the mass ratio [A / B] of the (meth)acrylic resin particles A to the water-soluble (meth)acrylic resin B was set to the mass ratio shown in Table 3, to obtain coating compositions with a solid content concentration of 43.5 mass%.
[0139] Comparative Example 9 An aqueous dispersion of (meth)acrylic resin particles A was obtained by performing the same operation as in the production method of (meth)acrylic resin particles A in Example 6. Next, an aqueous dispersion of other (meth)acrylic resin particles C was obtained by performing the same operation as in the production method of (meth)acrylic resin particles A in Example 6, except that the monomer composition of the (meth)acrylic resin particles was changed to the monomer composition shown in Table 4. Next, 300.0 parts by mass (137.1 parts by mass as solids) of the aqueous dispersion of (meth)acrylic resin particles A and 48.1 parts by mass (15.2 parts by mass as solids) of the aqueous dispersion of other (meth)acrylic resin particles C were mixed, and then an appropriate amount of deionized water was added to obtain a coating composition with a solids concentration of 43.5% by mass.
[0140] Comparative Example 10 An aqueous dispersion of (meth)acrylic resin particles A was obtained by performing the same operation as in the method for producing (meth)acrylic resin particles A in Example 6. Next, an aqueous dispersion of other (meth)acrylic resin particles C was obtained by performing the same operation as in the method for producing (meth)acrylic resin particles A in Example 6, except that the monomer composition of the (meth)acrylic resin particles was changed to the monomer composition shown in Table 4. Next, 300.0 parts by mass (137.1 parts by mass as solids) of the aqueous dispersion of (meth)acrylic resin particles A and 105.0 parts by mass (34.3 parts by mass as solids) of the aqueous dispersion of other (meth)acrylic resin particles C were mixed, and an appropriate amount of deionized water was added to obtain a coating composition with a solids concentration of 43.5% by mass.
[0141] The monomer composition (unit: mass%), glass transition temperature (Tg) (unit: °C), and average primary particle size (unit: nm) of the (meth)acrylic resin particles A in Examples 1 to 21 and Comparative Examples 1 to 10 are shown in Tables 1 to 4. The glass transition temperature of the (meth)acrylic resin particles A was measured by the same method as the above-mentioned method for measuring the glass transition temperature of the specific (meth)acrylic resin particles A. The average primary particle size of the (meth)acrylic resin particles A was measured by the same method as the above-mentioned method for measuring the average primary particle size of the specific (meth)acrylic resin particles A.
[0142] The monomer compositions (unit: mass%) and weight average molecular weights (Mw) of the water-soluble (meth)acrylic resins B in Examples 1 to 21 and Comparative Examples 1 to 8 are shown in Tables 1 to 3. The weight average molecular weights of the water-soluble (meth)acrylic resins B were measured by the same method as the method for measuring the weight average molecular weight of the water-soluble (meth)acrylic resin B described above.
[0143] For the water-soluble (meth)acrylic resins B in Examples 1 to 21 and Comparative Examples 1 to 8, the haze values of the resin films were measured by the method already described, and all were confirmed to be 3.0 or less, i.e., to be water-soluble (meth)acrylic resins.
[0144] The monomer composition (unit: mass%), glass transition temperature (Tg) (unit: °C), and average primary particle size (unit: nm) of the other (meth)acrylic resin particles C in Comparative Examples 9 and 10 are shown in Table 4. The glass transition temperature of the other (meth)acrylic resin particles C was measured by the same method as that for measuring the glass transition temperature of the specific (meth)acrylic resin particles A described above. The average primary particle size of the other (meth)acrylic resin particles C was measured by the same method as that for measuring the average primary particle size of the specific (meth)acrylic resin particles A described above.
[0145] [Measurement of gel fraction of coating composition] The gel fraction of the coating compositions of Examples 1 to 21 and Comparative Examples 1 to 10 was measured by the same method as the method for measuring the gel fraction of the coating composition of the present disclosure described above. Specifically, the measurement was performed as follows.
[0146] (1) Preparation of Resin Film with Release Film (1-1) Gel Fraction of Coating Composition at 170°C The coating composition was applied to a 100-µm-thick polyethylene terephthalate (PET) release film using a 4-mil (101.6 µm) applicator to form a coating film. The formed coating film was then dried at room temperature (25°C) for 24 hours and then further dried at 170°C for 90 seconds to obtain Resin Film X with Release Film.
[0147] (1-2) Gel fraction of coating composition at 200°C The coating composition was applied to a 100-µm-thick polyethylene terephthalate (PET) release film using a 4-mil (101.6 µm) applicator to form a coating film. The formed coating film was then dried at room temperature (25°C) for 24 hours, and then further dried at 170°C for 90 seconds, and then at 200°C for 60 seconds to obtain a resin film Y with a release film.
[0148] (2) Measurement of gel fraction Using the obtained resin film X with a release film and resin film Y with a release film, the operations from [2] onwards in the method for measuring the gel fraction of the coating composition of the present disclosure were carried out. The measurement results are shown in Tables 1 to 4.
[0149] [Evaluation] The coating compositions of Examples 1 to 21 and Comparative Examples 1 to 10 were evaluated as follows.
[0150] 1. Coatability A 2 cm x 10 cm electrical steel sheet (product number: 30HX1600, manufactured by Nippon Steel Corporation) was prepared. A coating composition diluted to a solids concentration of 32% by mass was applied to the surface of the prepared electrical steel sheet to a wet film thickness of 6.25 μm. The applied coating composition was then dried by heating at 170°C for 90 seconds using a hot air circulation dryer. The dried film was observed using an optical microscope to confirm the presence and extent of cissing and cracking. Evaluation was then performed according to the following evaluation criteria. The evaluation results are shown in Tables 1 to 4. In the evaluation criteria below, "AA," "A," and "B" indicate practical levels, with "B" being preferred, "A" being more preferred, and "AA" being even more preferred.
[0151] -Evaluation criteria- AA: No cissing or cracking was observed. A: Very slight cissing was observed, but no cracking was observed. B: Slight cissing and cracking was observed, but at a level that would not pose a problem in practical use. C: Obvious cissing and cracking was observed, and at a level that would pose a problem in practical use.
[0152] 2. High-Temperature Adhesion Strength Two 2 cm x 10 cm electromagnetic steel sheets (product number: 30HX1600, manufactured by Nippon Steel Corporation) were prepared. A coating composition diluted to a solids concentration of 32% by mass was applied to the surfaces of the two prepared electromagnetic steel sheets so that the film thickness after drying was 2 μm. The applied coating composition was then heated and dried at 170°C for 90 seconds using a hot air circulation dryer to prepare an evaluation sample. The two evaluation samples prepared were arranged so that the overlapping area was 2 cm x 2 cm, and thermocompression bonding was performed (temperature: 200°C, time: 60 seconds, pressure: 3 MPa). A tensile shear bond strength test was performed on the thermocompression-bonded evaluation sample in an environment of 150°C. The tensile shear bond strength test was performed in accordance with JIS K 6852:1994. Based on the measured adhesive strength (also referred to as "high-temperature adhesive strength"), evaluation was carried out in accordance with the following evaluation criteria. The measured values and evaluation results are shown in Tables 1 to 4. In the evaluation criteria below, "AA", "A", and "B" are practically acceptable levels, with "B" being preferred, "A" being more preferred, and "AA" being even more preferred.
[0153] -Evaluation criteria- AA: The shear adhesive strength was 0.60 MPa or more. A: The shear adhesive strength was in the range of 0.40 MPa or more and less than 0.60 MPa. B: The shear adhesive strength was in the range of 0.20 MPa or more and less than 0.40 MPa. C: The shear adhesive strength was in the range of less than 0.20 MPa.
[0154] 3. Pot life Immediately after production, 300 ml of the coating composition was placed in a plastic bottle (a so-called polyethylene container), sealed, and then allowed to stand for 2 days in an environment at an ambient temperature of 25°C. After standing, the viscosity of the coating composition at 25°C was measured using a BH-type viscometer (model number: BH II, manufactured by Toki Sangyo Co., Ltd.). The obtained value was compared with the viscosity value of the coating composition immediately after production, which was measured in advance, and evaluation was performed according to the following evaluation criteria. The evaluation results are shown in Tables 1 to 4. In the following evaluation criteria, "A" indicates a level that is practically usable.
[0155] -Evaluation criteria- A: There was no change in the viscosity of the coating composition even after 2 days had passed since production. B: There was a change in the viscosity of the coating composition within 2 days after production.
[0156]
[0157]
[0158]
[0159]
[0160] Details of each monomer listed in Tables 1 to 4 are as follows: <Monomer having a self-crosslinking group> "NMAM": N-methylolacrylamide "NBMA": N-butylolacrylamide "GMA": glycidyl methacrylate <Monomer having a self-crosslinking group and a hydroxyl group> "HEAA": hydroxyethylacrylamide <Monomer having a carboxyl group> "MAA": methacrylic acid "AA": acrylic acid <Monomer having a hydroxyl group> "2HEMA": 2-hydroxyethyl methacrylate <(meth)acrylic acid alkyl ester monomer> "n-BA": n-butyl acrylate "MMA": methyl methacrylate "2EHA": 2-ethylhexyl acrylate "EA": ethyl acrylate <Other monomers> "St": styrene "HDDA": 1,6-hexanediol diacrylate "AAM": acrylamide
[0161] In Tables 1 to 4, "-" in the column of monomer composition means that the corresponding monomer is not used. In Tables 1 to 4, the values in the column of monomer composition are all solid content equivalent values.
[0162] The results shown in Tables 1 to 4 demonstrate that the coating compositions of the present disclosure have superior coatability compared to the coating compositions of the comparative examples. It also demonstrates that the coating compositions of the present disclosure can form coating films that exhibit high adhesive strength even at high temperatures of 200°C. Furthermore, it also demonstrates that the coating compositions of the present disclosure have excellent pot life.
[0163] The disclosure of Japanese Patent Application No. 2023-163623, filed on September 26, 2023, is incorporated herein by reference in its entirety. All documents, patent applications, and technical standards described herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard was specifically and individually indicated to be incorporated by reference.
Claims
1. A coating composition for laminated steel sheets, comprising: (meth)acrylic resin particles A having a glass transition temperature of 55°C or higher, a water-soluble (meth)acrylic resin B; and water, the ratio of the mass content of the (meth)acrylic resin particles A to the mass content of the water-soluble (meth)acrylic resin B being 95 / 5 to 85 / 15.
2. A coating composition for laminated steel sheets according to claim 1, wherein the water-soluble (meth)acrylic resin B contains a structural unit derived from a monomer having a self-crosslinking group.
3. A coating composition for laminated steel sheets according to claim 1 or 2, wherein the water-soluble (meth)acrylic resin B contains a structural unit derived from a monomer having a hydroxyl group.
4. A coating composition for laminated steel sheets according to claim 1 or 2, wherein the average primary particle size of the (meth)acrylic resin particles A is 250 nm to 450 nm.
5. A coating composition for laminated steel sheets according to claim 1 or 2, wherein the monomer having a self-crosslinking group in the (meth)acrylic resin particles A is at least one selected from the group consisting of N-methylolacrylamide (NMAM), N-butyrolacrylamide (NBMA), hydroxyethylacrylamide (HEAA), and glycidyl methacrylate (GMA).
6. A coating composition for laminated steel plates according to claim 1 or 2, wherein the content of structural units derived from the monomer having a self-crosslinking group in the water-soluble (meth)acrylic resin B is 0.1 mass % to 10.0 mass % relative to the total structural units of the water-soluble (meth)acrylic resin B.
7. A coating composition for laminated steel plates according to claim 1 or 2, wherein the content of structural units derived from the monomer having a hydroxyl group in the water-soluble (meth)acrylic resin B is 5% by mass to 30% by mass relative to the total structural units of the water-soluble (meth)acrylic resin B.