Chemically strengthened glass-ceramic, cover glass, electronic device and glass component
Patent Information
- Application Number
- MYPI2026004810
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-05-13
- Filing Date
- 2025-05-13
- Publication Date
- 2025-11-13
AI Technical Summary
Existing chemically strengthened lithium disilicate microcrystalline glass exhibits improved mechanical properties but reduced environmental durability and weather resistance after increasing the sodium content on the surface. This results in surface roughness, fogging, whitening, and spots, affecting the user experience and display effect.
By controlling the surface composition and stress structure of chemically strengthened glass-ceramics, ensuring that N = n*(CT_LD-50000)/10000 is within the range of -32.5 < N < 15, and by combining specific crystal phase structures and glass composition, the stress layer depth and stress value are optimized to achieve high stress levels and good weather resistance.
While maintaining high mechanical strength, it improves the environmental durability and weather resistance of chemically strengthened microcrystalline glass, prevents surface roughness, fogging and spotting problems, and enhances the user experience and display effect.
Smart Images

Figure PI2026004810_DRAWING_001 
Figure PI2026004810_DRAWING_002 
Figure PI2026004810_DRAWING_003
Abstract
Description
Chemically strengthened glass-ceramics, cover glass, electronic device and glass article
[0001] Cross Reference to Related Applications
[0002] This application claims priority to the Chinese patent application entitled "Chemically strengthened glass-ceramics, cover glass, electronic device and glass article" filed on May 13, 2024 with the China National Intellectual Property Office, having the application number 202410590891.4, the content of which is incorporated herein by reference in its entirety. TECHNICAL FIELD
[0003] The present application relates to the technical field of glass-ceramics, in particular, to a chemically strengthened glass-ceramics, cover glass, electronic device and glass article. BACKGROUND
[0004] Glass-ceramics is a kind of solid composite material formed by controlled crystallization of base glass during heat treatment. Glass-ceramics contains microcrystalline phase and glass phase. Compared with ordinary glass materials without microcrystalline phase, glass-ceramics generally has higher strength, because the microcrystalline phase has higher strength than the glass phase, absorbs more energy when breaking, and can also extend the crack propagation path and hinder crack propagation, thus consuming more impact energy during the breaking and crushing process.
[0005] In recent years, glass-ceramics have been gradually applied to various electronic devices, such as mobile phones, watches, tablets, notebook computers, e-book readers or other similar devices, as cover glasses for electronic devices, such as display screen cover glasses and electronic device back cover glasses. For the display screen of electronic devices, the cover glass is generally required to have good optical performance, as well as a relatively thin thickness, high mechanical performance, good environmental durability or weather resistance, etc.
[0006] In order to further improve the mechanical performance of glass-ceramics, chemical strengthening treatment is usually required for glass-ceramics, and ion exchange is performed to produce chemically strengthened glass-ceramics with high stress level, high mechanical strength performance and high damage resistance.
[0007] For glass-ceramics with lithium disilicate as the main crystalline phase, the main ion exchange performed during chemical strengthening is usually sodium-lithium ion exchange, i.e., sodium ions in the chemical strengthening molten salt bath are ion exchanged with lithium ions in the glass-ceramics during chemical strengthening. In order to obtain chemically strengthened glass-ceramics with high mechanical performance, a certain amount of sodium ions are usually exchanged into the glass-ceramics to achieve high stress level by using the volume difference of exchanged ions, thereby improving the mechanical strength performance. If the content of exchanged sodium ions is low, the mechanical strength performance cannot be improved.
[0008] It should be noted that this part of the present application only provides the background of the present application, and does not necessarily constitute the prior art or the known art. SUMMARY
[0009] When the lithium disilicate as the main crystal phase of the glass-ceramics is subjected to sodium-lithium exchange during the chemical strengthening process, the deep compressive stress and the depth of the compressive stress layer of the glass-ceramics can be improved, but the surface of the glass-ceramics after exchange is prone to form a sodium-rich layer. When the exchange leads to an increase in the sodium content on the surface of the chemically strengthened glass-ceramics, the mechanical properties can be improved, but the high sodium content on the surface can easily cause the environmental durability or weather resistance of the chemically strengthened glass-ceramics to decrease. Generally, when the chemically strengthened glass-ceramics with a high sodium content on the surface is used in a sweat erosion environment for a long time or after being used in a humid environment, the smoothness of the surface of the chemically strengthened glass-ceramics can easily decrease and become rough. More seriously, the chemically strengthened glass-ceramics can become foggy, and spots or white marks that cannot be wiped off can be formed on the surface. These situations not only reduce the feeling of the user touching the screen, but also significantly reduce the screen display effect and appearance of the chemically strengthened glass-ceramics. Moreover, if the spots and fogging or whitening problem occurs at the position of the camera, it will also seriously affect the camera effect of the mobile phone.
[0010] The purpose of the present application is to provide a chemically strengthened glass-ceramics with a high stress level, which can ensure high mechanical strength performance and good environmental durability or weather resistance, by making the surface composition and stress of the chemically strengthened glass-ceramics with lithium disilicate as the main crystal phase meet a specific relationship.
[0011] In order to achieve the above-mentioned purpose, the present application provides the following technical solutions:
[0012] In a first aspect, a chemically strengthened glass-ceramics is provided, which contains a lithium disilicate crystal phase, wherein the lithium disilicate crystal phase has a larger mass percentage than other crystal phases present in the chemically strengthened glass-ceramics; the chemically strengthened glass-ceramics has a compressive stress layer on the surface and a tensile stress in the interior; and the chemically strengthened glass-ceramics satisfies:
[0013] N = n * (CT_LD-50000) / 10000, -32.5 < N < 15, preferably -28.0 ≤ N ≤ 0, more preferably -20.0 ≤ N ≤ -2.5,
[0014] wherein n = (mass percentage of Na2O on the surface of the chemically strengthened glass-ceramics / mass percentage of K2O on the surface of the chemically strengthened glass-ceramics) 2The surface Na2O mass percentage of the chemically strengthened glass-ceramics and the surface K2O mass percentage of the chemically strengthened glass-ceramics are determined by XRF; CT_LD is the linear density of tensile stress, in MPa / mm, and the data are substituted into the formula N according to the above unit requirements to obtain the calculation results, and the unit is not involved in the calculation.
[0015] The present application makes the chemically strengthened glass-ceramics meet the requirements of the specific crystal structure and the formula N, so that the chemically strengthened glass-ceramics can achieve good weather resistance while meeting the high stress level, and can better meet the market application requirements of the chemically strengthened glass-ceramics.
[0016] As an optional embodiment, the chemically strengthened glass-ceramics meet: 45000 MPa / mm≤CT_LD≤52000 MPa / mm, preferably 45900 MPa / mm≤CT_LD≤50000 MPa / mm, and more preferably 47500 MPa / mm≤CT_LD≤50000 MPa / mm.
[0017] By making the chemically strengthened glass-ceramics meet the appropriate stress structure, it is beneficial to obtain a chemically strengthened glass-ceramics product with a higher stress level, and further beneficial to play the improvement effect of the stress structure on the mechanical strength performance, so as to ensure that the chemically strengthened glass-ceramics meet excellent damage resistance.
[0018] As an optional embodiment, the value of the formula N is -2.52, -4.07, -4.47, -4.75, -10.59, -11.90 or -12.73; and / or
[0019] The value of CT_LD is 47517.24 MPa / mm, 48185.39 MPa / mm, 49692.43 MPa / mm, 47636.26 MPa / mm, 47919.69 MPa / mm, 47679.19 MPa / mm or 48097.14 MPa / mm.
[0020] As an optional embodiment, the surface Na2O mass percentage of the chemically strengthened glass-ceramics is 5% to 8.5% in terms of mass percentage of oxides, preferably 5.5% to 7.5%, as determined by XRF; and / or,
[0021] The surface K2O mass percentage of the chemically strengthened glass-ceramics is 0.7% to 2.0% in terms of mass percentage of oxides, preferably 0.7% to 1.5%, as determined by XRF; and / or,
[0022] The chemical strengthening glass-ceramics has a Na2O content of 3% to 3.5% by mass at the center or in the composition of the tensile stress layer, preferably a Na2O content of 3.1% to 3.2% by mass.
[0023] As an optional embodiment, the chemical strengthening glass-ceramics has a surface Na2O content of 5.30%, 6.12%, 7.00%, 5.21%, 6.32%, 5.17% or 6.36% by mass as determined by XRF; and / or,
[0024] As an optional embodiment, the chemical strengthening glass-ceramics has a surface K2O content of 1.25%, 0.81%, 0.77%, 1.24%, 0.80% or 1.26% by mass as determined by XRF; and / or,
[0025] The chemical strengthening glass-ceramics has a Na2O content of 3.16% or 3.14% by mass at the center or in the composition of the tensile stress layer.
[0026] As an optional embodiment, the chemical strengthening glass-ceramics satisfies:
[0027] Y = ΔC × ((CT_LD-50000) / 100) 2 Y < 60, preferably Y ≤ 50, more preferably Y ≤ 20,
[0028] wherein ΔC is the difference between the surface Na2O content of the chemical strengthening glass-ceramics and the Na2O content at the center of the chemical strengthening glass-ceramics, the surface Na2O content being determined by XRF; CT_LD is the tensile stress linear density in MPa / mm, in formula Y, the data is substituted into the formula in the above unit and the calculation result is obtained, and the unit is not involved in the calculation.
[0029] By making the chemical strengthening glass-ceramics satisfy the specific crystal structure and the requirement of formula Y, it is beneficial to make the chemical strengthening glass-ceramics achieve a high stress level.
[0030] As an optional embodiment, the value of formula Y is 0.36, 10.14, 11.58, 11.88, 13.02, 13.25 or 14.84.
[0031] As an optional embodiment, the chemical strengthening glass-ceramics satisfies:
[0032] 75MPa≤|CT_AV|≤120MPa, preferably 77MPa≤|CT_AV|≤90MPa, wherein |CT_AV| is the absolute value of the average tensile stress; and / or,
[0033] DOL_0 is 0.18t-0.25t, preferably 0.20t-0.25t, wherein DOL_0 is the depth of compressive stress layer, t is the thickness of the chemically strengthened glass-ceramic; and / or
[0034] CS_50 is 150MPa-250MPa, preferably 160MPa-180MPa, wherein CS_50 refers to the compressive stress value at the depth of 50μm from the main surface of the chemically strengthened glass-ceramic.
[0035] By making the chemically strengthened glass-ceramic satisfy the suitable stress structure, it is beneficial to obtain the chemically strengthened glass-ceramic product with higher stress level, and further beneficial to exert the improvement effect of the stress structure on the mechanical strength performance, to ensure that the chemically strengthened glass-ceramic satisfies excellent damage resistance performance.
[0036] As an optional embodiment, the composition at the center or the tensile stress layer of the chemically strengthened glass-ceramic comprises, in terms of mole percentage of oxides: SiO2: 61.50%-63.40%, Al2O3: 2.75%-2.99%, P2O5: 0.91%-1.91%, ZrO2: 4.20%-4.85%, Na2O: 1.80%-3.20%, B2O3: 0-1.00%, and Li2O: 25.32%-26.52%.
[0037] By satisfying the specific glass composition, it is beneficial to obtain the glass-ceramic satisfying the specific crystal phase structure, and beneficial to obtain the chemically strengthened glass-ceramic satisfying the specific stress structure.
[0038] As an optional embodiment, the composition at the center or the tensile stress layer of the chemically strengthened glass-ceramic comprises, in terms of mole percentage of oxides:
[0039] The mole percentage of SiO2 is 61.50%-63.30%, preferably the mole percentage of SiO2 is 62.00%-62.60%; and / or,
[0040] The mole percentage of P2O5 is 1.20%-1.91%, preferably the mole percentage of P2O5 is 1.30%-1.60%; and / or,
[0041] The mole percentage of Na2O is 1.85%-3.05%, preferably the mole percentage of Na2O is 2.20%-3.00%; and / or,
[0042] B2O3 is 0-0.65% in mole; and / or, ZrO2 is 4.20-4.60% in mole; and / or,
[0043] Li2O is 25.52-26.52% in mole, preferably, Li2O is 25.52-26.00% in mole.
[0044] As an optional embodiment, in the composition of the center or the tensile stress layer of the chemically strengthened glass-ceramics, in mole percentage of oxide:
[0045] SiO2 is 63.26%, 62.35% or 62.52% in mole; and / or,
[0046] Al2O3 is 2.87%, 2.94% or 2.92% in mole; and / or,
[0047] P2O5 is 1.41% or 1.53% in mole; and / or,
[0048] ZrO2 is 4.33% or 4.34% in mole; and / or,
[0049] Na2O is 2.36%, 2.93% or 2.96% in mole; and / or,
[0050] Li2O is 25.77%, 25.91% or 25.73% in mole.
[0051] As an optional embodiment, in the composition of the center or the tensile stress layer of the chemically strengthened glass-ceramics, the mole percentage of Na2O [Na2O], the mole percentage of B2O3 [B2O3] and the mole percentage of ZrO2 [ZrO2] satisfy the following relationship:
[0052] Z = -1.344 x (2.65-100 x [Na2O])2+ 0.466 x 100 x [B2O3] + 1.203 x 100 x [ZrO2], 4.80≤Z≤5.35, preferably, 5.05≤Z≤5.25;
[0053] and / or,
[0054] In the composition of the center or the tensile stress layer of the chemically strengthened glass-ceramics, the mole percentage of Na2O [Na2O] and the mole percentage of B2O3 [B2O3] satisfy the following relationship:
[0055] 0.90%≤ [Na2O] - [B2O3] ≤ 3.10%, preferably, 2.00%≤ [Na2O] - [B2O3] ≤ 3.00%, more preferably, 2.30%≤ [Na2O] - [B2O3] ≤ 3.00%; and / or,
[0056] The molar percentage of Na2O [Na2O] and the molar percentage of Li2O [Li2O] in the composition at the center of the chemically strengthened glass-ceramic or in the tensile stress layer satisfy the following relationship:
[0057] 8.55≤ [Li2O] / [Na2O] ≤ 13.85, preferably, 8.60≤ [Li2O] / [Na2O] ≤ 11.00.
[0058] As an alternative embodiment, the composition at the center of the chemically strengthened glass-ceramic or in the tensile stress layer satisfies:
[0059] the value of Z is 5.10, 5.09 or 5.12; and / or,
[0060] the value of [Na2O] - [B2O3] is 2.36%, 2.93% or 2.96%; and / or,
[0061] the value of [Li2O] / [Na2O] is 10.92, 8.84 or 8.69.
[0062] As an alternative embodiment, the lithium disilicate crystalline phase has a mass fraction of more than 70% of all the crystalline phases of the chemically strengthened glass-ceramic,
[0063] Preferably, the lithium disilicate crystalline phase has a mass fraction of more than 85% of all the crystalline phases of the chemically strengthened glass-ceramic.
[0064] As an alternative embodiment, the average grain size of the chemically strengthened glass-ceramic is 40 nm or less, preferably, the average grain size is 15 nm to 35 nm; and / or,
[0065] The crystallinity of the chemically strengthened glass-ceramic is more than 45%; preferably, the crystallinity of the chemically strengthened glass-ceramic is 45% to 85%, more preferably, the crystallinity of the chemically strengthened glass-ceramic is 55% to 65%.
[0066] As an alternative embodiment, the chemically strengthened glass-ceramic is transparent in the visible wavelength range, preferably, the transmittance of the chemically strengthened glass-ceramic is ≥ 90.00% for a 550 nm wavelength light at a thickness of 0.70 mm, preferably, the transmittance is > 90.40%; and / or,
[0067] at a thickness of 0.70 mm, the chemically strengthened glass-ceramics has a haze of <0.30%, preferably a haze of <0.20%, and / or,
[0068] at a thickness of 0.70 mm, the chemically strengthened glass-ceramics has a b value of <0.70, preferably a b value of <0.60.
[0069] As an optional embodiment, the chemically strengthened glass-ceramics has a Young's modulus of >100 GPa, preferably the chemically strengthened glass-ceramics has a Young's modulus of 105 GPa to 112.50 GPa; and / or
[0070] the chemically strengthened glass-ceramics has a Vickers hardness of >650 kgf / mm 2 , preferably the chemically strengthened glass-ceramics has a Vickers hardness of 650 kgf / mm 2 to 800 kgf / mm 2 .
[0071] As an optional embodiment, the chemically strengthened glass-ceramics is planar or curved; and / or, the chemically strengthened glass-ceramics has a thickness of 0.3 mm to 2 mm, preferably 0.45 mm to 0.8 mm; and / or, the chemically strengthened glass-ceramics does not contain a petalite crystal phase.
[0072] As an optional embodiment, the chemically strengthened glass-ceramics is subjected to a high temperature and high humidity failure test at a temperature of 85°C and a relative humidity of 85%, and has a high temperature and high humidity failure time of >240 h, wherein the high temperature and high humidity failure time is the total time length from the start of the high temperature and high humidity test to the appearance of spots or whitening marks on the chemically strengthened glass-ceramics that cannot be wiped off.
[0073] In a second aspect, a cover glass is provided, which is made of the chemically strengthened glass-ceramics according to any one of the embodiments of the first aspect, and the cover glass comprises the chemically strengthened glass-ceramics according to any one of the embodiments of the first aspect.
[0074] In a third aspect, an electronic device is provided, which comprises the chemically strengthened glass-ceramics according to any one of the embodiments of the first aspect.
[0075] As an optional embodiment, the electronic device comprises a housing assembled on the outer side of the electronic device, and the housing comprises the chemically strengthened glass-ceramics according to any one of the embodiments of the first aspect.
[0076] As an optional embodiment, the housing comprises a display screen cover plate assembled on the front side of the electronic device, and the display screen cover plate comprises the chemically strengthened glass-ceramics according to any one of the embodiments of the first aspect.
[0077] As an optional embodiment, the shell comprises a back cover assembled at the back side of the electronic device, and the back cover comprises the chemically strengthened microcrystalline glass according to any one of the embodiments of the first aspect.
[0078] As an optional embodiment, the electronic device further comprises a camera assembly located inside the shell, and the shell comprises a camera protection cover plate covering the camera assembly, and the camera protection cover plate comprises the chemically strengthened microcrystalline glass according to any one of the embodiments of the first aspect.
[0079] As an optional embodiment, the electronic device further comprises a middle frame, and the middle frame comprises the chemically strengthened microcrystalline glass according to any one of the embodiments of the first aspect.
[0080] In some embodiments, the shell can be partially made of the chemically strengthened microcrystalline glass or entirely made of the chemically strengthened microcrystalline glass. The electronic device in the present application can be one or more of the display screen cover plate, the back cover, the camera protection cover plate, and the middle frame, which are made of the chemically strengthened microcrystalline glass according to any one of the embodiments of the first aspect.
[0081] In a fourth aspect, a glass device is provided, which comprises the chemically strengthened microcrystalline glass according to any one of the embodiments of the first aspect.
[0082] Compared with the prior art, one or more of the above technical solutions provided in the present application have the following advantages:
[0083] The present application makes the surface composition and stress structure of the chemically strengthened microcrystalline glass with lithium disilicate as the main crystal phase meet a specific relationship, so that the chemically strengthened microcrystalline glass can achieve good weather resistance while meeting a high stress level, and better meet the market application requirements. BRIEF DESCRIPTION OF DRAWINGS
[0084] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings needed in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of the present application, and therefore should not be considered as limiting the scope. For those skilled in the art, other related drawings can also be obtained without creative labor.
[0085] FIG. 1 is an XRD pattern of the microcrystalline glass of Example 1.
[0086] FIG. 2 is a comparison diagram of the transmittance curves of the microcrystalline glass and the chemically strengthened microcrystalline glass of Example 1 in the 360 nm-740 nm wavelength band.
[0087] Figure 3 is a comparison chart of XRD patterns of the microcrystalline glass and the chemically strengthened microcrystalline glass of Example 1.
[0088] Figure 4 is a schematic diagram of a front side structure of an electronic device according to an embodiment of the present application.
[0089] Figure 5 is a schematic diagram of a rear side structure of an electronic device according to an embodiment of the present application.
[0090] Figure 6 is a schematic diagram of a structure of an electronic device according to an embodiment of the present application.
[0091] Figure 7 is a comparison chart of the chemically strengthened microcrystalline glass of Example 1 before and after high temperature and high humidity test, wherein (7a) is the chemically strengthened microcrystalline glass before high temperature and high humidity test, and (7b) is the chemically strengthened microcrystalline glass taken out after 10 days of high temperature and high humidity test.
[0092] Figure 8 is a comparison chart of the chemically strengthened microcrystalline glass of Example 2 before and after high temperature and high humidity test, wherein (8a) is the chemically strengthened microcrystalline glass before high temperature and high humidity test, and (8b) is the chemically strengthened microcrystalline glass taken out after 10 days of high temperature and high humidity test.
[0093] Figure 9 is a comparison chart of the chemically strengthened microcrystalline glass of Example 3 before and after high temperature and high humidity test, wherein (9a) is the chemically strengthened microcrystalline glass before high temperature and high humidity test, and (9b) is the chemically strengthened microcrystalline glass taken out after 10 days of high temperature and high humidity test.
[0094] Figure 10 is a comparison chart of the chemically strengthened glass of Comparative Example 1 before and after high temperature and high humidity test, wherein (10a) is the chemically strengthened microcrystalline glass before high temperature and high humidity test, and (10b) is the chemically strengthened microcrystalline glass taken out after 10 days of high temperature and high humidity test.
[0095] Figure 11 is a comparison chart of the chemically strengthened glass of Comparative Example 2 before and after high temperature and high humidity test, wherein (11a) is the chemically strengthened microcrystalline glass before high temperature and high humidity test, and (11b) is the chemically strengthened microcrystalline glass taken out after 10 days of high temperature and high humidity test.
[0096] Reference signs: 1 - housing; 11 - display cover plate; 12 - rear cover; 13 - camera protection cover plate; 2 - camera assembly; 3 - middle frame; 4 - display module. DETAILED DESCRIPTION
[0097] The embodiments of the present application will be described in detail below with examples, but those skilled in the art will understand that the following examples are only for illustration of the present application and should not be regarded as limiting the scope of the present application. The specific conditions are not specified in the examples, and the conventional conditions or the conditions recommended by the manufacturer are used. The reagents or instruments used are not specified by the manufacturer, and are conventional products that can be obtained by commercial purchase.
[0098] The endpoints of the ranges and any values disclosed herein are not limited to the precise values stated. The endpoints of the ranges and the values are approximate values and include values approximating these. For ranges, the endpoints are combined with the language "between" to indicate "between but not including" the endpoints. Thus, ranges include the endpoints. For ranges, the endpoints are combined with the language "up to," to indicate "up to, but not including" the endpoint. Thus, ranges include the endpoint. For ranges, the endpoints are combined with the language "at least," to indicate "at least, but not more than" the endpoint. Thus, ranges include the endpoint. For ranges, the endpoints are combined with the language "no more than," to indicate "no more than, but not including" the endpoint. Thus, ranges include the endpoint. For ranges, the endpoints are combined with the language "less than," to indicate "less than, but not including" the endpoint. Thus, ranges include the endpoint. For ranges, the endpoints are combined with the language "greater than," to indicate "greater than, but not including" the endpoint. Thus, ranges include the endpoint. For ranges, the endpoints are combined with the language "greater than or equal to," to indicate "greater than or equal to, but not including" the endpoint. Thus, ranges include the endpoint. For ranges, the endpoints are combined with the language "less than or equal to," to indicate "less than or equal to, but not including" the endpoint. Thus, ranges include the endpoint. The terms "optionally", "optional", and other similar phrases as used herein are intended to mean that the indicated feature may or may not be present. The term "and / or" as used herein is intended to represent any possible combination of the words "and" and "or". Thus, for example, "A and / or B" means A and B are both present, or A is present alone, or B is present alone, or A and B are both not present.
[0099] Terminology and test methods:
[0100] In the present application, the glass-ceramics are a kind of solid composite materials containing both glass phase and crystal phase (or also called microcrystalline phase, crystalline phase) prepared by targeted and controlled heat treatment of the base glass. The glass-ceramics are also called glass ceramics or crystallized glass or crystalline glass.
[0101] In the present application, the chemically strengthened glass-ceramics are solid composite materials obtained by chemical strengthening treatment of the glass-ceramics. It should be understood that, during the chemical strengthening treatment, the alkali metal ions with large ionic radius (such as potassium ions or sodium ions) in the molten salt bath (or also called molten salt bath) will replace the alkali metal ions with small ionic radius (such as sodium ions or lithium ions) in the glass-ceramics, thereby generating an exchange ion volume difference and generating a compressive stress (or also called compression stress) on the surface of the glass-ceramics.
[0102] In the present application, the base glass refers to the glass that has not been subjected to nucleation treatment, crystallization treatment and strengthening treatment, or also called base glass.
[0103] In the present application, the composition at the center of the chemically strengthened glass-ceramics refers to the composition at or near the center of the depth or thickness of the chemically strengthened glass-ceramics, that is, the composition of the region in the chemically strengthened glass-ceramics that has not been subjected to ion exchange. It should be understood that the composition at the center of the chemically strengthened glass-ceramics is the same as or substantially the same as the composition of the glass-ceramics used to prepare the chemically strengthened glass-ceramics but has not been subjected to chemical strengthening treatment.
[0104] In the present application, the visible light wavelength range refers to 360 nm to 740 nm.
[0105] In the present application, haze refers to the percentage of the intensity of transmitted light deviating from incident light by 2.5° or more in the total intensity of transmitted light.
[0106] In the present application, the main crystal phase (or also referred to as the primary crystal phase) refers to a crystal phase having a higher weight content (or also referred to as a weight percentage, a mass percentage) than other crystal phases present in the glass-ceramic or the chemically strengthened glass-ceramic.
[0107] In the present application, the main surface refers to the surface having the largest surface area, such as the upper surface or the lower surface of a horizontally placed glass-ceramic sheet.
[0108] In the present application, the crystallinity refers to the percentage of the total mass of the crystal phase or the crystal in the glass-ceramic or the chemically strengthened glass-ceramic in the mass of the glass-ceramic or the chemically strengthened glass-ceramic, or also referred to as the total content of the crystal phase in the glass-ceramic or the chemically strengthened glass-ceramic.
[0109] In the present application, when light of a certain wavelength is irradiated to the main surface of the glass-ceramic or the chemically strengthened glass-ceramic, the light will be reflected, absorbed and transmitted, and the ratio of the intensity of the transmitted portion to the intensity of the incident light is the transmittance.
[0110] In the present application, the D65 light source is a light source for measuring the color of an object irradiated with daylight containing the ultraviolet region, having a color temperature of 6500 K and a color rendering index Ra higher than 90, and showing a wide spectral distribution in the visible wavelength region.
[0111] In the present application, the crystallized glass raw material refers to a glass raw material that is heat treated for a period of time to reach a certain crystallinity, but has not yet reached the target crystallinity, and can continue to crystallize to reach the target crystallinity by being heated.
[0112] In the present application, CT_LD refers to the tensile stress linear density, with the unit of MPa / mm. It should be understood that after the glass-ceramic is placed in a molten salt bath for ion exchange, a compressive stress layer (or also referred to as a compressive stress layer) is formed on the surface of the glass-ceramic, and a tensile stress layer (or also referred to as a tensile stress layer) is formed in the interior of the glass-ceramic. In the present application, during the chemical strengthening process, the alkali metal ions with a larger radius in the molten salt bath are ion exchanged with the alkali metal ions with a smaller radius in the glass-ceramic, thereby forming a compressive stress layer on the surface of the glass-ceramic and a tensile stress layer in the interior of the glass-ceramic, that is, a chemically strengthened glass-ceramic containing a compressive stress layer and a tensile stress layer is prepared. In the present application, CT_LD is calculated by the following formula:
[0113] Wherein, t is the thickness of the chemically strengthened glass-ceramics, in mm; DOL_0 is the depth of the compressive stress layer of the chemically strengthened glass-ceramics, in μm; |CT_AV| is the absolute value of the average tensile stress of the chemically strengthened glass-ceramics, in MPa. It should be understood that the formula for calculating the tensile stress line density is calculated by substituting the data into the above unit requirements, and the calculation result is obtained, and the unit does not participate in the calculation.
[0114] In the present application, CS_50 refers to the compressive stress value at a depth of 50 μm from the main surface of the chemically strengthened glass-ceramics, in MPa, which is obtained by SLP-2000 stress meter testing.
[0115] In the present application, |CT_AV| refers to the absolute value of the average tensile stress, in MPa, specifically the absolute value of the average of all tensile stresses in the tensile stress layer, which is obtained by SLP-2000 stress meter testing.
[0116] In the present application, DOL_0 refers to the depth of the compressive stress layer, or the depth of the compressive stress layer, specifically the distance from any main surface of the chemically strengthened glass-ceramics to the position close to the surface where the compressive stress is zero, which is obtained by SLP-2000 stress meter testing.
[0117] In the present application, the test method of the aforementioned stress performance is as follows: when testing CS_50, DOL_0, |CT_AV| of the chemically strengthened glass-ceramics using SLP-2000 stress meter, the relevant parameters of the stress meter are set as follows: light source wavelength is 518 nm, SOC (photoelastic coefficient) is set to 26 [(nm / cm) / MPa], refractive index is set to 1.56, and exposure time is set to 300 μsec. After measuring DOL_0 and |CT_AV|, the tensile stress line density (CT_LD) value of the chemically strengthened glass-ceramics is calculated by the aforementioned formula for calculating the tensile stress line density.
[0118] In the present application, the value of b is used to represent the yellow-blue value of the material. The b value in the present application is the transmitted light b value, and a positive b value indicates that the material is blue.
[0119] In the present application, Vickers hardness refers to a standard for indicating the hardness of a material proposed by Robert L. Smith and George E. Sandland of Vickers Ltd in 1921.
[0120] In the present application, the testing method of Vickers hardness is as follows: the glass-ceramics or the chemically strengthened glass-ceramics is made into a small piece with a length, width and thickness of 50 mm x 50 mm x 0.70 mm, and a glass sample with a clean surface and no visible scratches, pits and cracks is selected as a test sample, and then a Vickers hardness tester is used to measure the Vickers hardness. The Vickers hardness tester used in the present application is a digital small load Vickers hardness tester with a model number of VTD405 from Beijing Kewei Technology Co., Ltd. The test conditions are as follows: load 300 gf, loading time 10 s, and the validity of the indentation meets the standard of GB / T 37900-2019 Ultra-thin glass hardness and fracture toughness test method Small load Vickers hardness indentation method. Three different positions on the surface of the same test sample are selected for measurement, and the average value of the three measurement results is taken as the Vickers hardness result of the test sample.
[0121] In the present application, the Young's modulus is used to characterize the ability of the glass to resist elastic deformation caused by external force. In the present application, the UMS-100 ultrasonic material characterization system is used to test the Young's modulus of the glass-ceramics by acoustic waves.
[0122] In the present application, the nucleation treatment refers to the formation of stable crystal nuclei in the base glass by heat treatment, and the crystallization treatment refers to the precipitation of crystals or crystalline phases in the base glass by heat treatment.
[0123] In the present application, the thickness of the glass-ceramics or the chemically strengthened glass-ceramics is measured by a micrometer. It should be understood that in the thickness direction, the degree of ion exchange changes from the surface to the center, and the total Na-K and / or Li-Na exchange amount increment (mass) is generally not more than 1.5% of the total mass of the sample, so the expansion effect in the thickness direction is extremely slight, and the thickness can be approximately considered as unchanged. That is, the thickness of the glass-ceramics changes very little before and after chemical strengthening, and can be basically ignored, and the thickness of the glass-ceramics is basically the same as that of the chemically strengthened glass-ceramics.
[0124] In the present application, the size of the glass-ceramics piece is measured by a two-dimensional measuring machine (instrument model number Miyu MY-YXCL-4030).
[0125] In the present application, the crystal phase, crystallinity and average grain size of the glass-ceramics or the chemically strengthened glass-ceramics are confirmed by XRD testing. The specific method is as follows:
[0126] (1) XRD test: The microcrystalline glass or chemically strengthened microcrystalline glass of the present application is crushed and ground into a sample with a particle size of less than 75 μm, and the ground sample is tested by an X-ray diffractometer to obtain an XRD diffraction peak curve and XRD diffraction data. The X-ray diffractometer used in the present application is Shimadzu XRD-6100, the target material is copper, 2θ = 10°-50°, the scanning speed is 6° / min, the working voltage is 40 kV, and the working current is 30 mA.
[0127] (2) Determination of crystal phase: The XRD diffraction data is analyzed by Jade software (JADE Standard 8.6) to determine the crystal phase in the sample.
[0128] (3) Determination of crystallinity: The test results (RAW format) of XRD are imported into Jade software for fitting and calculation, so that the crystallinity of the sample can be determined.
[0129] (4) Determination of average grain size: The result data obtained by XRD test can be used to calculate the average grain size (or also called average crystal size) of the sample according to the Scherrer formula D = Kλ / (βcosθ). Wherein, λ is the X-ray wavelength, λ = 0.154056 nm, β is the half-height width of the diffraction peak, K = 0.89, and θ is the Bragg diffraction angle. Specifically, the RAW format file output by the XRD instrument is curve-fitted in Jade software, and the fitting report is output by Jade. According to the angle 2θ value and Peak FWHM value corresponding to each diffraction peak in the fitting report, the Peak FWHM value is converted to radian: β = (FWHM / 180×3.14), and the grain size of each diffraction peak is calculated by the Scherrer formula D = Kλ / (βcosθ) and then averaged to obtain the average grain size in the sample.
[0130] In the present application, the transmittance, haze and b value of the microcrystalline glass are tested by a haze meter according to the national standard GB / T 7962.12-2010 Test methods for colourless optical glasses Part 12: Spectral transmission. Specifically, the transmittance, haze and b value of light with different wavelengths are tested by a haze meter for 5 pieces of microcrystalline glass in the same batch. The average of the b values and the haze values measured for the 5 pieces of microcrystalline glass are recorded as the b value result and the haze result of the microcrystalline glass, respectively. The average of the transmittance values measured at 550 nm wavelength light for the 5 pieces of microcrystalline glass is recorded as the transmittance result of the microcrystalline glass at 550 nm wavelength light. The haze meter used in the present application is Konica Minolta Spectrophotometer CM-3600A, the light receiving optical system is transmission, the spectral method is plane diffraction grating, the wavelength range is 360 nm-740 nm, the wavelength interval is 10 nm, the illumination light source is pulse xenon lamp x 4, the environmental temperature for placing the instrument is 24℃, and the air humidity is 40%.
[0131] In the present application, the anti-sandpaper drop height of each sample in the same embodiment or the same comparative example is added, and the value obtained by dividing the number of samples is recorded as the average anti-sandpaper drop height of the tested chemically strengthened glass-ceramics, which is used to characterize the drop damage resistance of the chemically strengthened glass-ceramics. Specifically, at least 10 samples are taken from each batch for testing, and the average anti-sandpaper drop height of each batch is calculated according to the following formula:
[0132] wherein n is the number of glass samples tested in each batch, and hi is the anti-sandpaper drop height of a single sample.
[0133] The test method for the anti-sandpaper drop height of a single sample is as follows:
[0134] Step 1: 80-mesh sandpaper is attached to the lower surface of a model machine with a weight of 181 g, and the model machine is placed on a green chart LT-SKDL-CD type drop machine.
[0135] Step 2: A chemically strengthened glass-ceramics sample to be tested with a length, width and thickness of 50 mm x 50 mm x 0.7 mm is placed directly below the model machine, with the chemically strengthened glass-ceramics sample facing the sandpaper. The model machine is dropped at a certain drop height to impact the chemically strengthened glass-ceramics sample directly below. If the chemically strengthened glass-ceramics sample does not break, the drop height of the model machine is increased at a certain rate, and the model machine is continued to be dropped to impact the chemically strengthened glass-ceramics sample directly below until the chemically strengthened glass-ceramics sample breaks. For example, the drop height of the model machine is started from 0.4 m, and the sample is dropped once. If the sample does not break, the drop height of the model machine is increased by 0.1 m, and the sample is dropped again. The above process is repeated until the chemically strengthened glass-ceramics sample breaks.
[0136] Step 3: The last drop height before the chemically strengthened glass-ceramics sample breaks is recorded as its anti-sandpaper drop height. For example, if the drop height is increased by 0.1 m each time, and the sample breaks at a drop height of 0.5 m, then the anti-sandpaper drop height of the sample is 0.4 m.
[0137] In the present application, the test method of the surface Na2O mass percentage of the chemically strengthened glass-ceramics is as follows: the content of Na element on the surface of the chemically strengthened glass-ceramics is measured by an X-ray fluorescence spectrometer (XRF), and then the surface Na2O mass percentage is calculated. The equipment model used is (Thermo Scientific ARL PERFORM’X), the target material is Rh (rhodium), the light tube voltage is 30 kV, the current is 80 mA, the collimator is 0.40, the crystal is selected as AxO3, the detector is selected as FPC, the test range is a circle with a diameter of 29 mm, and the test method is X_UQ method in OXSAS analysis software.
[0138] In the present application, the test method of the surface K2O mass percentage of the chemically strengthened glass-ceramics is as follows: the content of K element on the surface of the chemically strengthened glass-ceramics is measured by an X-ray fluorescence spectrometer (XRF), and then the surface K2O mass percentage is calculated. The equipment model used is (Thermo Scientific ARL PERFORM’X), the target material is Rh (rhodium), the light tube voltage is 40 kV, the current is 60 mA, the collimator is 0.15, the crystal is selected as LiF200, the detector is selected as FPC, the test range is a circle with a diameter of 29 mm, and the test method is X_UQ method in OXSAS analysis software.
[0139] In the present application, the XRF test uses a non-standard test, and the concentration of elements or oxides with atomic number 6 or less in the chemically strengthened glass-ceramics is not tested. During the test, the chemically strengthened glass-ceramic sheet is directly cut into a suitable size (such as 34 mm*34 mm), placed flat in the sample box, and covered with the test aperture for testing.
[0140] In the present application, the high temperature and high humidity failure time of the chemically strengthened glass-ceramics is tested under the condition of a test temperature of 85°C and a relative humidity of 85%, i.e. a high temperature and high humidity failure test is performed, and the weather resistance of the chemically strengthened glass-ceramics is characterized by the high temperature and high humidity failure test result. The high temperature and high humidity failure time is the total time from the start of the high temperature and high humidity test to the appearance of spots or whitish marks that cannot be wiped off in the chemically strengthened glass-ceramics.
[0141] In the present application, the high temperature and high humidity failure time of the chemically strengthened microcrystalline glass is mainly tested whether it can be greater than 240h (10 days). Specifically: the chemically strengthened microcrystalline glass sample is placed in a temperature and humidity alternating test chamber with a temperature of 85℃ and a relative humidity of 85%, and the initial sample placement time is recorded. Then every 24h, the chemically strengthened microcrystalline glass sample is taken out, the surface of the removed chemically strengthened microcrystalline glass sample is wiped with a dust-free cloth, and whether there are spots and / or whitening marks that cannot be wiped off in the sample are observed. If there are no spots and / or whitening marks that cannot be wiped off in the sample, it is continued to be placed in the temperature and humidity alternating test chamber, waiting for the next sampling observation. If after 240h of sample placement test, the chemically strengthened microcrystalline glass sample still does not appear spots and / or whitening marks that cannot be wiped off, it is indicated that it has passed the high temperature and high humidity test, and is in OK state, recorded as qualified. The high temperature and high humidity failure time of the chemically strengthened microcrystalline glass is greater than 240h. If after 240h of sample placement test or less than 240h of sample placement, spots and / or whitening marks that cannot be wiped off are observed in the sample, it is indicated that the chemically strengthened microcrystalline glass has not passed the high temperature and high humidity test, and is in NG state, recorded as unqualified. The high temperature and high humidity failure time of the chemically strengthened microcrystalline glass is less than 240h. The temperature and humidity alternating test chamber used in the present application is QTH_80C full temperature and humidity alternating test chamber.
[0142] Without being limited by any theory, when the lithium disilicate microcrystalline glass with lithium disilicate crystal phase as the main crystal phase is chemically strengthened, mainly sodium-lithium ion exchange is carried out, which can improve the deep compressive stress and compressive stress layer depth of the glass. However, after the exchange, the microcrystalline glass is easy to form a sodium-rich layer on the surface of the glass. If the surface sodium content is too high, the environmental durability (or also known as weather resistance) of the prepared chemically strengthened microcrystalline glass will be poor. After long-term use in sweat or after passing through a humid environment, the surface smoothness of the chemically strengthened microcrystalline glass product will decrease, the surface will become rough, and more seriously, it will be foggy or whitish, or form spots that cannot be wiped off. Such problems not only reduce the user's touch feeling on the screen, but also reduce the display effect and appearance of the glass screen. Moreover, if the spots, fog, or whitening occur at the camera position, it will also seriously affect the camera effect of the mobile phone and reduce the service life of the equipment. However, if the surface sodium content of the chemically strengthened (ion exchange) chemically strengthened microcrystalline glass is too low, the compressive stress formed by sodium-lithium ion exchange will be relatively low, thereby leading to a relatively low mechanical strength of the chemically strengthened microcrystalline glass, which cannot meet the use requirements.
[0143] In view of this, in order to enable the chemically strengthened microcrystalline glass to maintain high stress and excellent mechanical strength performance while taking into account good weather resistance, the present application provides a chemically strengthened microcrystalline glass with good weather resistance and high stress. The present application provides a chemically strengthened microcrystalline glass with a higher stress level, which can ensure higher mechanical strength performance, while having good environmental durability or weather resistance, by making the surface composition and stress of the chemically strengthened microcrystalline glass with lithium disilicate as the main crystal phase satisfy a specific relationship. Understandably, the surface composition can be the material composition or component distribution of the surface of the substrate glass, microcrystalline glass or chemically strengthened microcrystalline glass, can also be the mass percentage of a certain component, the molar percentage of a certain component, the mass percentage relationship between two or more than two material components, the mass content relationship between two or more than two material components, can also be the molar content relationship between two or more than two material components, can also be a combination of the foregoing, and the like. For example: the mass percentage of Na2O on the surface of the chemically strengthened microcrystalline glass or the mass percentage of K2O on the surface of the chemically strengthened microcrystalline glass, for example: the content relationship between Na2O on the surface of the chemically strengthened microcrystalline glass and K2O on the surface of the chemically strengthened microcrystalline glass, for example: the mass percentage relationship between Na2O on the surface of the chemically strengthened microcrystalline glass and K2O on the surface of the chemically strengthened microcrystalline glass.
[0144] In some embodiments of the present application, a chemically strengthened microcrystalline glass is provided, which contains lithium disilicate crystal phase, wherein the lithium disilicate crystal phase has a larger mass percentage than other crystal phases present in the chemically strengthened microcrystalline glass; the chemically strengthened microcrystalline glass has a compressive stress layer on the surface and a tensile stress in the interior; the chemically strengthened microcrystalline glass satisfies:
[0145] N = n * (CT_LD-50000) / 10000, -32.5 < N < 15, preferably, -28.0 ≤ N ≤ 0, more preferably, -20.0 ≤ N ≤ -2.5,
[0146] wherein n = (mass percentage of Na2O on the surface of the chemically strengthened microcrystalline glass / mass percentage of K2O on the surface of the chemically strengthened microcrystalline glass) 2 The mass percentage of Na2O on the surface of the chemically strengthened microcrystalline glass and the mass percentage of K2O on the surface of the chemically strengthened microcrystalline glass are determined by XRF; CT_LD is the tensile stress linear density, with units of MPa / mm; in the formula N, the data is substituted into the calculation according to the above unit requirements, and the calculation result is obtained, and the unit does not participate in the calculation.
[0147] Li2Si205crystal phase is an orthorhombic crystal based on [Si2O5] tetrahedral array, and the shape of the crystal is flat or plate-like. The presence of Li2Si205crystals in the interior of the glass-ceramics forces the path of a crack to twist as it passes through the crystals, thereby preventing the propagation of the crack and improving the strength and fracture toughness of the glass-ceramics. At the same time, the light refraction index of Li2Si205crystals is close to that of the glass matrix (e.g., the base glass used to prepare the glass-ceramics in the present application), which is an ideal crystal phase for preparing high-transparency glass-ceramics. In the present application, the glass-ceramics contain a structure in which Li2Si205is the main crystal phase, which is conducive to ensuring that they have high intrinsic strength (or also known as inherent strength) and excellent optical performance.
[0148] In the present application, by making the chemically strengthened glass-ceramics meet the requirements of the specific crystal phase structure and formula N, the chemically strengthened glass-ceramics can achieve good weather resistance while meeting high stress levels, and can better ensure that the chemically strengthened glass-ceramics meet application requirements.
[0149] In some embodiments, the value of formula N can be -30 to 10, -25 to 5, -20 to 0, -15 to -2, or -10 to -2.5, etc. In some embodiments, the value of formula N can be -32.5, -30, -28.4, -28, -26, -24, -22, -20, -18, -16, -14, -12, -10, -8, -6, -4, -2.5, -2, 0, 2, 4, 6, 8, 10, 12, 14, 15, -2.52, -4.07, -4.47, -4.75, -10.59, -11.90, or -12.73, or a value within a numerical range formed by any two of the above specific numerical values as end points, as long as a chemically strengthened glass-ceramic with the required performance of the present application can be obtained. It should be understood that in specific embodiments, any of the above ranges can be combined with any other range, as long as a chemically strengthened glass-ceramic with the required performance of the present application can be obtained.
[0150] In some embodiments of the present application, the chemically strengthened glass-ceramics meet the requirement: 45000 MPa / mm≤CT_LD≤52000 MPa / mm, preferably 45900 MPa / mm≤CT_LD≤50000 MPa / mm, and more preferably 47500 MPa / mm≤CT_LD≤50000 MPa / mm. By making the CT_LD of the chemically strengthened glass-ceramics not less than 45000 MPa / mm, it is conducive to ensuring that the tensile stress stored in the interior of the chemically strengthened glass-ceramics is sufficiently dense, thereby ensuring that it has a high surface stress level, and thereby facilitating the improvement of the stress structure on the mechanical strength performance, ensuring that it has excellent damage resistance, such as excellent rough surface drop damage resistance, to meet market demand.
[0151] In some embodiments, the CT_LD of the chemically strengthened glass-ceramics can be 45000 MPa / mm to 50000 MPa / mm, 45500 MPa / mm to 49500 MPa / mm, 46000 MPa / mm to 49000 MPa / mm, 46500 MPa / mm to 48500 MPa / mm, or 46000 MPa / mm to 48000 MPa / mm. In some embodiments, the CT_LD of the chemically strengthened glass-ceramics can be 45000 MPa / mm, 45900 MPa / mm, 46000 MPa / mm, 47000 MPa / mm, 47517.24 MPa / mm, 48185.39 MPa / mm, 49692.43 MPa / mm, 47636.26 MPa / mm, 47919.69 MPa / mm, 47679.19 MPa / mm, 48097.14 MPa / mm, 48000 MPa / mm, 49000 MPa / mm, 49700 MPa / mm, 50000 MPa / mm, 51000 MPa / mm, or 52000 MPa / mm, or a value within a range defined by any two of the foregoing specific values as endpoints, as long as a chemically strengthened glass-ceramics with desired properties of the present application is obtained. It should be understood that in specific embodiments, any of the foregoing ranges can be combined with any other range, as long as a chemically strengthened glass-ceramics with desired properties of the present application is obtained.
[0152] In some embodiments of the present application, the surface Na2O content of the chemically strengthened glass-ceramics is 5% to 8.5%, preferably 5.5% to 7.5%, in terms of mass percentage of oxide, as determined by XRF; and / or, in some embodiments of the present application, the surface K2O content of the chemically strengthened glass-ceramics is 0.7% to 2.0%, preferably 0.7% to 1.5%, in terms of mass percentage of oxide, as determined by XRF. By having the surface K element or the surface Na element of the chemically strengthened glass-ceramics satisfy a specific range, it is beneficial to achieve good weather resistance while obtaining a high stress level.
[0153] In some embodiments, the surface Na20 content of the chemically strengthened glass-ceramics can be 5%, 5.30%, 6.12%, 7.00%, 5.21%, 6.32%, 5.17%, 6.36%, 7%, 7.5%, 8%, or 8.5% by mass of oxide, or can be a value within a range defined by any two of the above specific values as endpoints, as long as a chemically strengthened glass-ceramic having the desired properties of the present application is obtained. It is understood that in specific embodiments, any of the above ranges can be combined with any other range, as long as a chemically strengthened glass-ceramic having the desired properties of the present application is obtained.
[0154] In some embodiments, the surface K20 content of the chemically strengthened glass-ceramics can be 0.7%, 1.25%, 0.81%, 0.77%, 1.24%, 0.80%, 1.26%, 1.5%, 1.8%, or 2.0% by mass of oxide, or can be a value within a range defined by any two of the above specific values as endpoints, as long as a chemically strengthened glass-ceramic having the desired properties of the present application is obtained. It is understood that in specific embodiments, any of the above ranges can be combined with any other range, as long as a chemically strengthened glass-ceramic having the desired properties of the present application is obtained.
[0155] In some embodiments of the present application, the Na20 content in the center or in the composition of the tensile stress layer of the chemically strengthened glass-ceramics is 3% to 3.5% by mass of oxide, preferably, the Na20 content is 3.1% to 3.2% by mass of oxide. It is understood that in the present application, the Na20 content in the center or in the composition of the tensile stress layer of the chemically strengthened glass-ceramics is 3% to 3.5%, which means that the Na20 content in the composition of the glass-ceramics or the base glass used to prepare the chemically strengthened glass-ceramics, which has not been subjected to chemical strengthening treatment, is 3% to 3.5%.
[0156] In some embodiments, the mass percentage of Na2O in the composition of the center or the tensile stress layer of the chemically strengthened glass-ceramics can be 3.1% to 3.4%, 3.1% to 3.3%, or 3% to 3.2%, in terms of mass percentage of oxides. In some embodiments, the mass percentage of Na2O in the composition of the center or the tensile stress layer of the chemically strengthened glass-ceramics can be 3%, 3.1%, 3.3%, 3.4%, 3.5%, 3.11%, 3.12%, 3.13%, 3.14%, 3.15%, 3.16%, 3.17%, 3.18%, 3.19%, or 3.2%, in terms of mass percentage of oxides, or can be a value within a value range with any two of the above specific values as endpoints, as long as a chemically strengthened glass-ceramics with desired properties in the present application can be obtained. It should be understood that in specific embodiments, any of the above ranges can be combined with any other range, as long as a chemically strengthened glass-ceramics with desired properties in the present application can be obtained.
[0157] In some embodiments of the present application, the concentration of Na ions in the chemically strengthened glass-ceramics varies at least in part of the compressive stress layer and reaches a minimum Na ion concentration at the contact with the tensile stress layer, and the chemically strengthened glass-ceramics satisfies:
[0158] Y = ΔC x ((CT_LD-50000) / 100) 2 Y < 60, preferably Y ≤ 50, more preferably Y ≤ 20,
[0159] wherein ΔC is the difference between the mass percentage of Na2O at the surface of the chemically strengthened glass-ceramics and the mass percentage of Na2O at the center of the chemically strengthened glass-ceramics, and the mass percentage of Na2O at the surface of the chemically strengthened glass-ceramics is determined by XRF; CT_LD is the tensile stress linear density, in units of MPa / mm, and in the formula Y, the data is calculated according to the above unit requirements, and the calculation result is obtained, and the unit does not participate in the calculation.
[0160] In the present application, by making the chemically strengthened glass-ceramics satisfy the requirements of specific crystal phase structure and formula Y, it is beneficial to make the chemically strengthened glass-ceramics achieve a high stress level.
[0161] In some embodiments, the value of Formula Y can be < 60, < 55, < 50, < 45, < 40, < 35, < 30, < 25, < 20, < 15, < 10, or < 5. In some embodiments, the value of Formula Y can be 0.1, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 22, 24, 26, 28, 30, 35, 40, 45, 50, 55, 60, 0.36, 10.14, 11.58, 11.88, 13.02, 13.25, or 14.84, or a value within a range between any two of the specifically mentioned values as endpoints, as long as the chemically strengthened glass with desired properties of the present application can be obtained. It should be understood that in specific embodiments, any of the above ranges can be combined with any other range, as long as the chemically strengthened glass with desired properties of the present application can be obtained.
[0162] In some embodiments of the present application, the chemically strengthened glass satisfies 75 MPa < |CT_AV| < 120 MPa, preferably 77 MPa < |CT_AV| < 90 MPa, where |CT_AV| is the absolute value of the average tensile stress. By keeping |CT_AV| of the chemically strengthened glass at a suitable level, it is beneficial to ensure that the chemically strengthened glass has a desired tensile stress layer distribution structure, and it is beneficial to ensure that it has a high surface stress level. A higher surface compressive stress level can offset more residual energy from a drop, crush, puncture, impact, or collision, and thus it is beneficial to ensure that the chemically strengthened glass has excellent damage resistance.
[0163] In some embodiments, |CT_AV| of the chemically strengthened glass can be 80 MPa to 115 MPa, 85 MPa to 110 MPa, 90 MPa to 105 MPa, or 93 MPa to 102 MPa. In some embodiments, |CT_AV| of the chemically strengthened glass can be 75 MPa, 80 MPa, 85 MPa, 90 MPa, 95 MPa, 100 MPa, 105 MPa, 110 MPa, 115 MPa, 120 MPa, 78.26 MPa, 79.83 MPa, 84.20 MPa, 79.01 MPa, 80.77 MPa, 77.61 MPa, or 79.23 MPa, or a value within a range between any two of the specifically mentioned values as endpoints, as long as the chemically strengthened glass with desired properties of the present application can be obtained. It should be understood that in specific embodiments, any of the above ranges can be combined with any other range, as long as the chemically strengthened glass with desired properties of the present application can be obtained.
[0164] In some embodiments of the present application, the chemically strengthened glass-ceramics satisfies: DOL_0 is 0.18t-0.25t, preferably, 0.20t-0.25t, wherein DOL_0 is the depth of compressive stress layer, and t is the thickness of the chemically strengthened glass-ceramics. By satisfying the appropriate proportional relationship between the depth of compressive stress layer and the thickness of the chemically strengthened glass-ceramics, it is beneficial to ensure that the chemically strengthened glass-ceramics is in a relatively optimal stress distribution state, and thus it is beneficial to exert the improvement effect of the stress structure on the mechanical strength performance.
[0165] In some embodiments, the value of DOL_0 / t of the chemically strengthened glass-ceramics can be 0.18, 0.19, 0.2, 0.21, 0.22, 0.23, 0.24 or 0.25, or can be a value within a numerical range constituted by any two of the above specific numerical values as endpoints, as long as the chemically strengthened glass-ceramics with the required performance of the present application can be obtained. It should be understood that in specific embodiments, any of the above ranges can be combined with any other range, as long as the chemically strengthened glass-ceramics with the required performance of the present application can be obtained.
[0166] In some embodiments of the present application, the chemically strengthened glass-ceramics satisfies: CS_50 is 150MPa-250MPa, preferably, 160MPa-180MPa, wherein CS_50 refers to the compressive stress value at a depth of 50μm from the main surface of the chemically strengthened glass-ceramics. By making the chemically strengthened glass-ceramics have a relatively high surface stress level, it can offset more residual energy of drop, extrusion, impact or collision, and thus it is beneficial to ensure that it has excellent damage resistance performance, such as excellent drop resistance performance.
[0167] In some embodiments, the CS_50 of the chemically strengthened glass-ceramics can be 150MPa, 160MPa, 170MPa, 180MPa, 190MPa, 210MPa, 220MPa, 230MPa, 240MPa, 250MPa, 162.81MPa, 166.33MPa, 170.25MPa, 165.17MPa, 169.43MPa, 167.89MPa, 170.28MPa or 200MPa, or can be a value within a numerical range constituted by any two of the above specific numerical values as endpoints, as long as the chemically strengthened glass-ceramics with the required performance of the present application can be obtained. It should be understood that in specific embodiments, any of the above ranges can be combined with any other range, as long as the chemically strengthened glass-ceramics with the required performance of the present application can be obtained.
[0168] It is understood that the chemically strengthened glass-ceramics of the present application are made from a glass-ceramic that is chemically strengthened, and unless over-ion exchanged, the composition and phase assemblage of the chemically strengthened glass-ceramic at a depth greater than the depth of compressive stress layer (DOL), such as at the center of the chemically strengthened glass-ceramic or the tensile stress layer, is the same or substantially the same as that of the glass-ceramic. The composition at the surface of the glass-ceramic article after chemical strengthening can be different from that of the glass-ceramic before chemical strengthening, which is due to the replacement of one type of alkali metal ion (e.g., Li + or Na + ) at the surface of the glass-ceramic by a larger alkali metal ion (e.g., Na + or K + ) during chemical strengthening. However, in embodiments, the glass composition and phase assemblage at or near the center of the depth or thickness of the glass-ceramic article remains the same as that of the as-formed glass-ceramic. That is, the composition (e.g., the composition of the tensile stress layer) and phase assemblage at the center of the chemically strengthened glass-ceramic of the present application is the same or substantially the same as that of the glass-ceramic that is not chemically strengthened.
[0169] In the present application, the glass-ceramic used to make the chemically strengthened glass-ceramic can be made from a base glass that is heat treated, and the base glass has the same or substantially the same composition as the glass-ceramic in terms of mole percent of oxides.
[0170] In some embodiments of the present application, the composition at the center or the tensile stress layer of the chemically strengthened glass-ceramic or the glass-ceramic used to make the chemically strengthened glass-ceramic or the base glass used to make the glass-ceramic comprises, in terms of mole percent of oxides, Si02: 61.50% to 63.40%, AI2O3: 2.75% to 2.99%, P2O5: 0.91% to 1.91%, Zr02: 4.20% to 4.85%, Na20: 1.80% to 3.20%, B203: 0 to 1.00%, and Li20: 25.32% to 26.52%. By satisfying the specific glass composition, it is beneficial to obtain a glass-ceramic that satisfies a specific crystalline phase structure, and it is beneficial to obtain a chemically strengthened glass-ceramic that satisfies a specific stress structure. In specific embodiments, any of the above ranges can be combined with any other range as long as the chemically strengthened glass-ceramic of the present application has the desired properties.
[0171] In the present application, SiO2 is an essential component for forming a glass network structure and is also one of the main components for forming lithium disilicate crystals. The higher the content of SiO2 in the glass system, the denser the network structure of the glass phase, and accordingly, the higher the mechanical strength of the glass-ceramics, the smaller the thermal expansion coefficient, and the better the heat resistance, dielectric properties and chemical stability. However, too high a content of SiO2 will result in a high melting temperature and a large melting viscosity of the base glass, increasing the difficulty of forming the base glass. When the content of SiO2 is too low, the weather resistance of the glass will decrease. Therefore, in order to balance the formability of the glass and the excellent properties, the molar percentage of SiO2 in the composition of the center of the chemically strengthened glass-ceramics or the composition of the tensile stress layer of the chemically strengthened glass-ceramics or the composition of the glass-ceramics used to prepare the chemically strengthened glass-ceramics or the composition of the base glass is 61.50% to 63.40%, preferably 61.50% to 63.30%, and more preferably 62.00% to 62.60%.
[0172] In some embodiments of the present application, the content of SiO2 in the composition of the center of the chemically strengthened glass-ceramics or the composition of the tensile stress layer of the chemically strengthened glass-ceramics or the composition of the glass-ceramics used to prepare the chemically strengthened glass-ceramics or the composition of the base glass can be 62.87%, 62.88%, 63.25%, 63.26%, 62.38%, 62.27%, 62.44%, 62.45%, 62.22%, 63.17%, 61.50%, 61.60%, 61.70%, 61.80%, 61.90%, 62.00%, 62.10%, 62.20%, 62.30%, 62.40%, 62.50%, 62.60%, 62.70%, 62.80%, 62.90%, 63.00%, 63.10%, 63.20%, 63.30%, 63.40%, 62.35%, or 62.52%, or a value within a range formed by any two of the above specific values as endpoints, as long as a glass-ceramics or a chemically strengthened glass-ceramics with the desired properties of the present application can be obtained. It should be understood that in specific embodiments, any of the above ranges can be combined with any other range, as long as a glass-ceramics or a chemically strengthened glass-ceramics with the desired properties of the present application can be obtained.
[0173] In the present application, Al2O3 is a component forming a glass network structure, and an appropriate amount of Al2O3 is beneficial to improve the chemical strengthening effect of the glass-ceramics, can improve the weather resistance of the glass, and to a certain extent, is beneficial to promote the ion exchange in the chemical strengthening process. However, an excessive amount of Al2O3 can increase the viscosity of the glass, and easily lead to the precipitation of other crystal phases, such as petalite, etc., which affects the crystal phase structure of the glass-ceramics. Therefore, in order to obtain the desired crystal phase structure and improve the chemical strengthening effect of the glass-ceramics, the molar percentage of Al2O3 in the composition of the center of the chemically strengthened glass-ceramics or the composition of the tensile stress layer or the composition of the glass-ceramics used to prepare the chemically strengthened glass-ceramics or the composition of the substrate glass is 2.75% to 2.99%.
[0174] In some embodiments of the present application, the content of Al2O3 in the composition of the center of the chemically strengthened glass-ceramics or the composition of the tensile stress layer or the composition of the glass-ceramics used to prepare the chemically strengthened glass-ceramics or the composition of the substrate glass, in terms of molar percentage of oxides, can be 2.75%, 2.77%, 2.79%, 2.81%, 2.83%, 2.85%, 2.86%, 2.87%, 2.89%, 2.91%, 2.93%, 2.94%, 2.95%, 2.97%, 2.99% or 2.92%, or can be a value within a value range formed by any two of the above specific values as endpoints, as long as a glass-ceramics or a chemically strengthened glass-ceramics with the required properties of the present application can be obtained. It should be understood that in specific embodiments, any of the above ranges can be combined with any other range, as long as a glass-ceramics or a chemically strengthened glass-ceramics with the required properties of the present application can be obtained.
[0175] In the present application, P2O5 acts as a nucleating agent and has the effect of promoting uniform nucleation of the glass. When the content of P2O5 is too low or too high, it will lead to poor crystallization effect, affect the optical properties of the obtained glass-ceramics, and reduce the transparency of the glass-ceramics. Therefore, in order to obtain the desired crystal phase structure and further achieve excellent optical properties and excellent mechanical strength properties, the molar percentage of P2O5 in the composition of the center of the chemically strengthened glass-ceramics or the composition of the tensile stress layer or the composition of the glass-ceramics used to prepare the chemically strengthened glass-ceramics or the composition of the substrate glass is 0.91% to 1.91%, preferably 1.20% to 1.91%, and more preferably 1.30% to 1.60%.
[0176] In some embodiments of the present application, the content of P2O5 in the composition of the center of the chemically strengthened glass-ceramics or the composition of the tensile stress layer of the chemically strengthened glass-ceramics or the composition of the glass-ceramics used for preparing the chemically strengthened glass-ceramics or the composition of the substrate glass can be 0.91%, 0.95%, 1.00%, 1.05%, 1.10%, 1.15%, 1.20%, 1.25%, 1.30%, 1.35%, 1.40%, 1.45%, 1.50%, 1.55%, 1.60%, 1.65%, 1.70%, 1.75%, 1.80%, 1.85%, 1.41%, 1.53%, 1.54% or 1.91% in terms of mole percentage of oxide, or can be a value within a range defined by any two of the above specific values as endpoints, as long as a glass-ceramics or a chemically strengthened glass-ceramics with desired properties of the present application can be obtained. It should be understood that in specific embodiments, any of the above ranges can be combined with any other range, as long as a glass-ceramics or a chemically strengthened glass-ceramics with desired properties of the present application can be obtained.
[0177] In the present application, ZrO2 is an intermediate oxide for glass formation, and an appropriate amount of ZrO2 can improve the chemical stability of the glass-ceramics, increase the hardness of the glass-ceramics and the scratch and drop resistance of the glass-ceramics, and improve the weather resistance of the glass. In addition, due to the high cation charge and strong field strength of ZrO2, it has a large accumulation effect on the glass structure and is often used as a nucleating agent in glass-ceramics. However, too high a content of ZrO2 can cause the glass to phase separate or be unfavorable for obtaining glass-ceramics with excellent optical properties. Therefore, in order to obtain glass-ceramics with excellent optical properties and high mechanical strength, the mole percentage of ZrO2 in the composition of the center of the chemically strengthened glass-ceramics or the composition of the tensile stress layer of the chemically strengthened glass-ceramics or the composition of the glass-ceramics used for preparing the chemically strengthened glass-ceramics or the composition of the substrate glass is 4.20% to 4.85%, preferably 4.20% to 4.60% in the present application.
[0178] In some embodiments of the present application, the content of Zr02in the composition of the center of the chemically strengthened glass-ceramics or the composition of the tensile stress layer of the chemically strengthened glass-ceramics or the composition of the glass-ceramics used to prepare the chemically strengthened glass-ceramics or the composition of the base glass can be 4.20%, 4.35%, 4.40%, 4.45%, 4.50%, 4.55%, 4.60%, 4.65%, 4.70%, 4.75%, 4.74%, 4.84%, 4.33%, 4.34%, 4.85% or 4.80% in terms of mole percent of oxide, or can be a value within a range defined by any two of the above specific values as endpoints, as long as a glass-ceramics or a chemically strengthened glass-ceramics with the desired properties of the present application can be obtained. It should be understood that in specific embodiments, any of the above ranges can be combined with any other range, as long as a glass-ceramics or a chemically strengthened glass-ceramics with the desired properties of the present application can be obtained.
[0179] In the present application, Na20 is an extra-network oxide, and an appropriate amount of Na20 can provide free oxygen, improve the viscosity of the glass, promote the melting and fining of the glass liquid, and also adjust the chemical strengthening rate. However, an excessive amount of Na20 not only reduces the crystallinity of the glass-ceramics, but also affects the chemical strengthening effect of the glass-ceramics. Therefore, in order to improve the formability of the base glass and the chemical strengthening effect of the glass-ceramics, the mole percent of Na20 in the composition of the center of the chemically strengthened glass-ceramics or the composition of the tensile stress layer of the chemically strengthened glass-ceramics or the composition of the glass-ceramics used to prepare the chemically strengthened glass-ceramics or the composition of the base glass is 1.80% to 3.20%, preferably 1.85% to 3.05%, and more preferably 2.20% to 3.00% in the present application.
[0180] In some embodiments of the present application, the content of Na2O in the composition of the center of the chemically strengthened glass-ceramics or the composition of the tensile stress layer of the chemically strengthened glass-ceramics or the composition of the glass-ceramics used for preparing the chemically strengthened glass-ceramics or the composition of the base glass can be 1.80%, 1.85%, 1.90%, 1.95%, 2.00%, 2.05%, 2.10%, 2.15%, 2.20%, 2.25%, 2.30%, 2.35%, 2.40%, 2.45%, 2.50%, 2.55%, 2.60%, 2.65%, 2.70%, 2.75%, 2.80%, 2.85%, 2.90%, 2.95%, 3.00%, 3.20%, 2.36%, 2.96%, 3.01%, 2.93% or 3.05% in terms of mole percentage, or can be a value within a range defined by any two of the above specific values as endpoints, as long as a glass-ceramics or a chemically strengthened glass-ceramics with desired properties of the present application can be obtained. It should be understood that in specific embodiments, any of the above ranges can be combined with any other range, as long as a glass-ceramics or a chemically strengthened glass-ceramics with desired properties of the present application can be obtained.
[0181] In the present application, B2O3 as a fluxing agent can reduce the high-temperature viscosity of the glass, improve the melting difficulty problem caused by ZrO2, and reduce the sag temperature of the glass, but excessive B2O3 can easily lead to a decrease in the transparency of the glass-ceramics. In addition, different structures can be formed at different contents of B2O3, which can have a great impact on the weather resistance of the glass, which is specifically manifested as follows: 3+ When the content of B2O3 is low, B 3+ The B ions are in [BO4] tetrahedrons, which reconnect the broken bonds in the glass caused by alkali metal ions, thereby helping to improve the weather resistance. With the increase of the content of B2O3, the structure of B 3+ ions is converted to [BO3] triangle, which instead leads to a decrease in weather resistance. Therefore, in order to improve the formability of the base glass and obtain a glass-ceramics with desired properties, the content of B2O3 in the composition of the center of the chemically strengthened glass-ceramics or the composition of the tensile stress layer of the chemically strengthened glass-ceramics or the composition of the glass-ceramics used for preparing the chemically strengthened glass-ceramics or the composition of the base glass is 0-1.00% in terms of mole percentage, preferably 0-0.65%.
[0182] In some embodiments of the present application, the content of B2O3 in the composition of the center of the chemically strengthened glass-ceramics or the composition of the tensile stress layer of the chemically strengthened glass-ceramics or the composition of the glass-ceramics used to prepare the chemically strengthened glass-ceramics or the composition of the base glass can be 0, 0.05%, 0.10%, 0.15%, 0.20%, 0.25%, 0.30%, 0.35%, 0.40%, 0.45%, 0.50%, 0.55%, 0.65%, 0.70%, 0.80%, 0.90%, 1.00% or 0.60% in terms of mole percent, or can be a value within a range defined by any two of the above specific values as endpoints, as long as a glass-ceramics or a chemically strengthened glass-ceramics with desired properties of the present application can be obtained. It should be understood that in specific embodiments, any of the above ranges can be combined with any other range, as long as a glass-ceramics or a chemically strengthened glass-ceramics with desired properties of the present application can be obtained.
[0183] In the present application, Li2O is an essential component to form the main crystalline phase of lithium disilicate crystalline phase, and is also an essential component to provide lithium ions for ion exchange during the chemical strengthening process. An appropriate amount of Li2O not only helps to improve the viscosity of the glass, promote the melting and fining of the glass liquid, but also helps to ensure that the desired content of lithium disilicate crystals is obtained, and at the same time, Li2O can also provide alkali lithium ions for ion exchange with large radius ions (such as sodium ions) in the molten salt bath, which is an important factor affecting the stress level that can be obtained by the chemically strengthened glass-ceramics. However, excessive Li2O will deteriorate the optical properties of the glass-ceramics. Therefore, in order to improve the formability of the base glass, obtain a microcrystalline glass with a desired structure, and at the same time improve the chemical strengthening effect of the glass-ceramics, the mole percent of Li2O in the composition of the center of the chemically strengthened glass-ceramics or the composition of the tensile stress layer of the chemically strengthened glass-ceramics or the composition of the glass-ceramics used to prepare the chemically strengthened glass-ceramics or the composition of the base glass is 25.32% to 26.52%, preferably 25.52% to 26.52%, and more preferably 25.52% to 26.00%.
[0184] In some embodiments of the present application, the content of Li2O in the composition of the center of the chemically strengthened glass-ceramics or the composition of the glass-ceramics used to prepare the chemically strengthened glass-ceramics or the composition of the substrate glass can be 25.32%, 25.52%, 25.60%, 25.65%, 25.70%, 25.75%, 25.80%, 25.85%, 25.90%, 25.95%, 26.00%, 26.05%, 26.10%, 26.15%, 26.20%, 26.25%, 26.30%, 26.35%, 26.40%, 26.45%, 25.62%, 25.82%, 25.69%, 25.36%, 25.77%, 25.87%, 25.79%, 26.03%, 25.74%, 26.52%, 25.91%, or 25.73% in terms of mole percent of the oxides, or can be a value within a value range formed by any two of the above specific values as endpoints, as long as a glass-ceramics or a chemically strengthened glass-ceramics with the desired properties of the present application can be obtained. It should be understood that in specific embodiments, any of the above ranges can be combined with any other range, as long as a glass-ceramics or a chemically strengthened glass-ceramics with the desired properties of the present application can be obtained.
[0185] Both Na2O and Li2O belong to alkali metal oxides, and they have the common feature of being able to destroy Si-O bonds in the glass, break the glass network, and reduce the high-temperature viscosity of the glass. However, if the amount added is too large, the weather resistance of the glass will be significantly impaired. The addition of multiple alkali metal oxides to the glass composition will produce a complex "synergistic effect", and the performance of the glass will not change linearly with the addition of a single alkali metal. This is called "mixed alkali effect", in which the weather resistance of the glass is improved by the addition of several alkali metal oxides to the glass composition, which is more beneficial than the addition of a single alkali metal oxide. However, there is also a certain limit, and too much or too little will make it difficult to obtain the desired effect.
[0186] In the present application, by adjusting and controlling the ratio relationship between the oxide components, especially the mole percent relationship between Na2O, B2O3, ZrO2, or Li2O, on the basis of adjusting and controlling the content range of each oxide component, it is beneficial to ensure that the glass-ceramics with the desired crystal structure is obtained, and it is also beneficial to ensure that the glass-ceramics has excellent optical properties and high intrinsic strength.
[0187] In some embodiments of the present application, the molar percentage of Na2O [Na2O], the molar percentage of B2O3 [B2O3] and the molar percentage of ZrO2 [ZrO2] in the composition of the center of the chemically strengthened glass-ceramics or the composition of the glass-ceramics used to prepare the chemically strengthened glass-ceramics or the composition of the base glass satisfy the following relationship:
[0188] Z = -1.344 x (2.65 - 100 x [Na2O])2+ 0.466 x 100 x [B2O3] + 1.203 x 100 x [ZrO2], 4.80 < Z < 5.35, preferably, 5.05 < Z < 5.25.
[0189] In some embodiments, the value of the molar percentage relationship Z between Na2O, B2O3 and ZrO2 in the composition of the center of the chemically strengthened glass-ceramics or the composition of the glass-ceramics used to prepare the chemically strengthened glass-ceramics or the composition of the base glass can be 4.80, 4.85, 4.90, 4.95, 4.98, 5.05, 5.06, 5.07, 5.08, 5.09, 5.10, 5.11, 5.12, 5.13, 5.14, 5.15, 5.16, 5.17, 5.18, 5.19, 5.35, 5.30 or 5.20, or can be a value within a numerical range formed by any two of the above specific numerical values as endpoints, as long as a glass-ceramics or a chemically strengthened glass-ceramics with the desired properties of the present application can be obtained. It should be understood that in specific embodiments, any of the above ranges can be combined with any other range, as long as a glass-ceramics or a chemically strengthened glass-ceramics with the desired properties of the present application can be obtained.
[0190] In some embodiments of the present application, the molar percentage of Na2O [Na2O] and the molar percentage of B2O3 [B2O3] in the composition of the center of the chemically strengthened glass-ceramics or the composition of the glass-ceramics used to prepare the chemically strengthened glass-ceramics or the composition of the base glass satisfy the following relationship: 0.90% < [Na2O] - [B2O3] < 3.10%, preferably, 2.00% < [Na2O] - [B2O3] < 3.00%, more preferably, 2.30% < [Na2O] - [B2O3] < 3.00%.
[0191] In some embodiments, the difference in mole percent between Na20 and B203, [Na20] - [B203], in the composition at the center of the chemically strengthened glass-ceramic or the composition of the glass-ceramic used to make the chemically strengthened glass-ceramic or the composition of the base glass, can be 0.90%, 1.00%, 1.20%, 1.25%, 1.26%, 1.35%, 1.45%, 1.55%, 1.65%, 1.75%, 1.85%, 1.95%, 2.00%, 2.05%, 2.15%, 2.25%, 2.35%, 2.45%, 2.50%, 2.55%, 2.65%, 2.75%, 2.85%, 2.95%, 3.10%, 1.79%, 0.96%, 2.36%, 2.96%, 3.01%, 2.93%, 3.00%, or 3.02%, or a value within a range having any two of these specific numerical values as endpoints, as long as a glass-ceramic or chemically strengthened glass-ceramic having the desired properties of the present application is obtained. It is understood that in specific embodiments, any of the above ranges can be combined with any other range, as long as a glass-ceramic or chemically strengthened glass-ceramic having the desired properties of the present application is obtained.
[0192] In some embodiments of the present application, the mole percent of Na20, [Na20], and the mole percent of Li20, [Li20], in the composition at the center of the chemically strengthened glass-ceramic or the composition of the glass-ceramic used to make the chemically strengthened glass-ceramic or the composition of the base glass, satisfy the following relationship: 8.55 < [Li20] / [Na20] < 13.85, preferably, 8.60 < [Li20] / [Na20] < 11.00.
[0193] In some embodiments, the ratio of the mole percent of Li20, [Li20], and the mole percent of Na20, [Na20], [Li20] / [Na20], in the composition at the center of the chemically strengthened glass-ceramic or the composition of the glass-ceramic used to make the chemically strengthened glass-ceramic or the composition of the base glass, can be 8.55, 9.00, 9.50, 10.00, 10.50, 10.55, 11.00, 11.50, 12.00, 12.50, 13.00, 13.50, 13.83, 10.93, 13.01, 10.92, 8.73, 8.61, 8.79, 8.83, 8.84, 8.69, or 13.85, or a value within a range having any two of these specific numerical values as endpoints, as long as a glass-ceramic or chemically strengthened glass-ceramic having the desired properties of the present application is obtained. It is understood that in specific embodiments, any of the above ranges can be combined with any other range, as long as a glass-ceramic or chemically strengthened glass-ceramic having the desired properties of the present application is obtained.
[0194] In some embodiments of the present application, the composition of the center of the chemically strengthened glass-ceramics or the composition of the glass-ceramics used to prepare the chemically strengthened glass-ceramics or the composition of the substrate glass, in addition to the above-mentioned composition ranges, can further include other components, as long as the glass-ceramics or the chemically strengthened glass-ceramics having the desired properties of the present application can be obtained. For example, in some embodiments, the composition of the center of the chemically strengthened glass-ceramics or the composition of the glass-ceramics used to prepare the chemically strengthened glass-ceramics or the composition of the substrate glass, in addition to the above-mentioned composition ranges, can further include, in terms of mole percent of oxides: CaO: 0.00-1.00 mol%; K2O: 0.00-1.00 mol%.
[0195] It should be understood that, in the present application, the crystalline structure of the glass-ceramics does not change significantly after the chemical strengthening treatment to obtain the chemically strengthened glass-ceramics, i.e., the crystallinity, average grain size, and optical properties of the glass-ceramics are the same as or substantially the same as those of the chemically strengthened glass-ceramics. For example, refer to the comparison in FIGS. 2 and 3. Similarly, it should be understood that the stress structure generated during the chemical strengthening process can appropriately improve the mechanical properties of the glass product. In the present application, the mechanical properties such as Young's modulus and Vickers hardness of the glass-ceramics do not decrease after the chemical strengthening treatment to obtain the chemically strengthened glass-ceramics, i.e., when the Young's modulus of the glass-ceramics is greater than 100 GPa, the Young's modulus of the chemically strengthened glass-ceramics obtained therefrom should also be greater than 100 GPa.
[0196] In the present application, "the lithium disilicate crystal phase has a greater mass percentage than other crystal phases present in the chemically strengthened microcrystalline glass" or "lithium disilicate as the main crystal phase" or other similar expressions refer to the lithium disilicate crystal phase accounts for more than 70 mass percent of all crystal phases of the microcrystalline glass or chemically strengthened microcrystalline glass according to the embodiments of the present application. In some embodiments, the mass of the lithium disilicate crystal phase accounts for more than 70% of all crystal phases of the microcrystalline glass used to prepare the chemically strengthened microcrystalline glass or the chemically strengthened microcrystalline glass, preferably, the mass of the lithium disilicate crystal phase accounts for more than 85% of all crystal phases of the microcrystalline glass used to prepare the chemically strengthened microcrystalline glass or the chemically strengthened microcrystalline glass. For example, the mass percentage (or also referred to as the weight percentage) of the lithium disilicate crystal phase in all crystal phases of the microcrystalline glass used to prepare the chemically strengthened microcrystalline glass or the chemically strengthened microcrystalline glass can be 70%, 79%, 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 96%, 97%, 98%, 100% or 95%, or a value within a value range formed by any two specific values as endpoints, as long as a microcrystalline glass or chemically strengthened microcrystalline glass with the required performance of the present application can be obtained. It should be understood that in specific embodiments, any of the above ranges can be combined with any other range, as long as a microcrystalline glass or chemically strengthened microcrystalline glass with the required performance of the present application can be obtained.
[0197] In some embodiments of the present application, the crystallinity of the microcrystalline glass or the chemically strengthened microcrystalline glass is more than 45%, preferably, the crystallinity of the microcrystalline glass or the chemically strengthened microcrystalline glass is 45% to 85%, more preferably, the crystallinity of the microcrystalline glass or the chemically strengthened microcrystalline glass is 55% to 65%. The higher the crystallinity of the microcrystalline glass or the chemically strengthened microcrystalline glass, the more conducive to obtaining high impact resistance and high intrinsic strength of the microcrystalline glass or the chemically strengthened microcrystalline glass. However, too high crystallinity not only affects the chemical strengthening effect of the microcrystalline glass, prolonging the chemical strengthening time of the microcrystalline glass to obtain a chemically strengthened microcrystalline glass with high stress level, but also affects the optical performance of the microcrystalline glass. In the present application, by making the microcrystalline glass meet the desired crystallinity, it is conducive to ensuring that the microcrystalline glass has excellent optical performance while meeting better impact resistance and high intrinsic strength, and at the same time, it is conducive to improving the chemical strengthening effect.
[0198] In some embodiments of the present application, the crystallinity of the glass-ceramic or the chemically strengthened glass-ceramic can be 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, or 85%, or can be a value within a range defined by any two of the above values as endpoints, as long as the glass-ceramic or the chemically strengthened glass-ceramic having the desired properties of the present application is obtained. It should be understood that in specific embodiments, any of the above ranges can be combined with any other range, as long as the glass-ceramic or the chemically strengthened glass-ceramic having the desired properties of the present application is obtained.
[0199] In some embodiments of the present application, non-limiting examples of other possible crystalline phases in the glass-ceramic or the chemically strengthened glass-ceramic include lithium phosphate crystalline phase. In some embodiments, it is preferred that the glass-ceramic or the chemically strengthened glass-ceramic does not contain petalite crystalline phase. "Does not contain petalite crystalline phase" herein includes a content of 0, or a content of no more than 0.1%. By controlling the precipitation of other crystalline phases, it is more beneficial to ensure that lithium disilicate forms the desired structure, thereby ensuring that the glass-ceramic or the chemically strengthened glass-ceramic obtains high mechanical strength performance, excellent optical performance, and excellent damage resistance performance.
[0200] In some embodiments of the present application, the average grain size of the glass-ceramic or the chemically strengthened glass-ceramic is 40 nm or less, preferably, the average grain size is 15-35 nm. A suitable average grain size is beneficial to make the glass-ceramic have excellent optical performance and high intrinsic strength, while if the average grain size is too high, the glass-ceramic is prone to devitrification, and the chemical strengthening effect will also be affected. In the present application, by making the glass-ceramic meet a suitable average grain size, it is beneficial to make the glass-ceramic have excellent optical performance while meeting better impact resistance performance and high intrinsic strength, and it is also beneficial to improve the chemical strengthening effect.
[0201] In some embodiments, the average grain size of the glass-ceramic or the chemically strengthened glass-ceramic can be 40 nm, 35 nm, 30 nm, 25 nm, 20 nm, 15 nm, or 10 nm, or can be a value within a range defined by any two of the above values as endpoints, as long as the glass-ceramic or the chemically strengthened glass-ceramic having the desired properties of the present application is obtained. It should be understood that in specific embodiments, any of the above ranges can be combined with any other range, as long as the glass-ceramic or the chemically strengthened glass-ceramic having the desired properties of the present application is obtained.
[0202] In some embodiments of the present application, the glass-ceramic or the chemically strengthened glass-ceramic is transparent in the visible wavelength range, preferably, the transmittance of the glass-ceramic or the chemically strengthened glass-ceramic is ≥ 90.00% for 550 nm wavelength light at a thickness of 0.70 mm, preferably the transmittance is > 90.40%. The chemically strengthened glass-ceramic satisfying the transmittance can ensure good light transmittance, good transparent effect, and is suitable for use in display screens with requirements for display effect. The "visible wavelength range" herein refers to light with a wavelength of 360 nm-740 nm.
[0203] In some embodiments, the transmittance of the glass-ceramic or the chemically strengthened glass-ceramic can be 90.00%, 90.10%, 90.20%, 90.31%, 90.40%, 90.50%, 91.00%, 90.52%, 90.70%, 90.62%, 90.85%, 90.70%, 90.63%, 90.51%, or 92.00% for 550 nm wavelength light at a thickness of 0.70 mm, or can be a value within a numerical range constituted by any two of the above specific numerical values as end points, as long as a glass-ceramic or a chemically strengthened glass-ceramic with the required performance of the present application can be obtained. It should be understood that in specific embodiments, any of the above ranges can be combined with any other range, as long as a glass-ceramic or a chemically strengthened glass-ceramic with the required performance of the present application can be obtained.
[0204] In some embodiments of the present application, the haze of the glass-ceramic or the chemically strengthened glass-ceramic is < 0.30% at a thickness of 0.70 mm. Haze is the cloudy or hazy appearance of the glass-ceramic or the chemically strengthened glass-ceramic inside or on the surface due to light diffusion, and the smaller the haze, the better the transparent effect and display effect of the glass-ceramic or the chemically strengthened glass-ceramic. In some embodiments, the haze of the glass-ceramic or the chemically strengthened glass-ceramic can be 0.25%, 0.20%, 0.15%, 0.10%, 0.05%, 0.21%, 0.14%, 0.13%, 0.15%, 0.16%, or 0.29% at a thickness of 0.70 mm, or can be a value within a numerical range constituted by any two of the above specific numerical values as end points, as long as a glass-ceramic or a chemically strengthened glass-ceramic with the required performance of the present application can be obtained. It should be understood that in specific embodiments, any of the above ranges can be combined with any other range, as long as a glass-ceramic or a chemically strengthened glass-ceramic with the required performance of the present application can be obtained.
[0205] In some embodiments of the present application, the b value of the glass-ceramic or chemically strengthened glass-ceramic is < 0.70, preferably ≤ 0.60 at a thickness of 0.70 mm. In the present application, the b value refers to the optical b value measured under D65 light source, and the Konica Minolta CM-3600A is used to measure the b value in the transmittance mode, and the result is shown as b (D65). The smaller the b value, the better the display effect of the glass-ceramic or chemically strengthened glass-ceramic can be ensured. When the b value is large, the glass-ceramic or chemically strengthened glass-ceramic will have an undesirable color, which will result in a display effect that cannot meet the application requirements of the display cover glass.
[0206] In some embodiments, the b value of the glass-ceramic or chemically strengthened glass-ceramic can be 0.69, 0.65, 0.60, 0.55, 0.50, 0.45, 0.40, 0.35, 0.30, 0.25, 0.48, 0.47, 0.52, 0.51, 0.54 or 0.20, or can be a value within a range formed by any two of the above specific values as endpoints, as long as the glass-ceramic or chemically strengthened glass-ceramic having the required properties of the present application can be obtained. It should be understood that in specific embodiments, any of the above ranges can be combined with any other range, as long as the glass-ceramic or chemically strengthened glass-ceramic having the required properties of the present application can be obtained.
[0207] The glass-ceramic or chemically strengthened glass-ceramic of the present application has high transmittance, low haze and low b value, which all indicate that the optical properties of the glass-ceramic or chemically strengthened glass-ceramic of the present application are excellent and have good uniformity, and the glass-ceramic or chemically strengthened glass-ceramic is in a transparent state, which can meet the application requirements of the display cover glass of electronic devices.
[0208] In some embodiments of the present application, the Young's modulus of the glass-ceramic or chemically strengthened glass-ceramic is ≥ 100 GPa, preferably the Young's modulus of the glass-ceramic or chemically strengthened glass-ceramic is 105 GPa to 112.50 GPa. By making the Young's modulus of the glass-ceramic or chemically strengthened glass-ceramic not less than 100 GPa, the high network structure strength of the glass-ceramic or chemically strengthened glass-ceramic can be ensured, the stress relaxation effect of the chemically strengthened glass-ceramic during ion exchange can be reduced, and the weakening effect of high temperature and long time factors on the deep stress in the compound compressive stress during ion exchange can be slowed down.
[0209] In some embodiments, the Young's modulus of the glass-ceramic or the chemically strengthened glass-ceramic can be 100 GPa, 105 GPa, 110 GPa, 106.32 GPa, 111.12 GPa, 110.82 GPa, 111.32 GPa, 111.09 GPa, 112.10 GPa, 111.51 GPa, or 112.50 GPa, or can be a value within a range defined by any two of the above specific values as endpoints, as long as the glass-ceramic or the chemically strengthened glass-ceramic having the desired properties of the present application can be obtained. It should be understood that in specific embodiments, any of the above ranges can be combined with any other range, as long as the glass-ceramic or the chemically strengthened glass-ceramic having the desired properties of the present application can be obtained.
[0210] In some embodiments of the present application, the Vickers hardness of the glass-ceramic or the chemically strengthened glass-ceramic is ≥ 650 kgf / mm 2 , preferably, the Vickers hardness of the glass-ceramic or the chemically strengthened glass-ceramic is 650 kgf / mm 2 ~ 800 kgf / mm 2 . The Vickers hardness of the glass-ceramic or the chemically strengthened glass-ceramic within the above range indicates that the glass-ceramic or the chemically strengthened glass-ceramic has high hardness and high intrinsic strength, thereby ensuring excellent mechanical properties.
[0211] In some embodiments of the present application, the Vickers hardness of the glass-ceramic or the chemically strengthened glass-ceramic can be 650 kgf / mm 2 , 654 kgf / mm 2 , 653 kgf / mm 2 , 658 kgf / mm 2 , 659 kgf / mm 2 , or 660 kgf / mm 2 , or can be a value within a range defined by any two of the above specific values as endpoints, as long as the glass-ceramic or the chemically strengthened glass-ceramic having the desired properties of the present application can be obtained. It should be understood that in specific embodiments, any of the above ranges can be combined with any other range, as long as the glass-ceramic or the chemically strengthened glass-ceramic having the desired properties of the present application can be obtained.
[0212] In some embodiments of the present application, the chemically strengthened glass-ceramic is subjected to high temperature and high humidity failure test under the condition of a temperature of 85°C and a relative humidity of 85%, and the high temperature and high humidity failure time of the chemically strengthened glass-ceramic is ≥ 240 h, wherein the high temperature and high humidity failure time is the total time from the start of the high temperature and high humidity test to the appearance of spots or whitish marks on the chemically strengthened glass-ceramic that cannot be wiped off.
[0213] The thickness of the glass-ceramic or chemically strengthened glass-ceramic can be selected by those skilled in the art according to the requirements. In some embodiments of the present application, the thickness of the glass-ceramic or chemically strengthened glass-ceramic is 0.3mm to 2mm, preferably 0.45mm to 0.8mm. Exemplarily, the thickness of the glass-ceramic or chemically strengthened glass-ceramic can be 0.3mm to 1.5mm, 0.3mm to 1.00mm or 0.40 to 0.80mm. In specific embodiments, any of the above ranges can be combined with any other range, as long as a chemically strengthened glass-ceramic with the required properties of the present application is obtained.
[0214] In some embodiments of the present application, the glass-ceramic or chemically strengthened glass-ceramic is planar or curved.
[0215] After the foregoing introduction of the composition, crystal phase structure and stress structure of the chemically strengthened glass-ceramic, the preparation method of the chemically strengthened glass-ceramic will be described in detail.
[0216] In the present application, the preparation process of the chemically strengthened glass-ceramic mainly includes the preparation process of the glass-ceramic and the chemical strengthening process, and the preparation process of the glass-ceramic mainly includes the preparation process of the base glass and the heat treatment process of the base glass.
[0217] In the present application, the base glass can be prepared by using the forming method in the prior art, and the present application does not have any limitation in this regard. For example, the forming method of the base glass can include but is not limited to float method, overflow method, calendering or casting process. Exemplarily, the components are mixed according to the formula, and after melting and forming, cooling and annealing treatment are performed, and the base glass is obtained.
[0218] Exemplarily, the raw materials (industrial conventional raw materials) are prepared according to the formula, a refining agent is added, and then the mixture is mixed for a period of time to obtain a raw material mixture with uniform mixture. The raw material mixture is placed in a platinum crucible, heated to 1250°C to 1680°C, preferably the melting temperature is 1480°C to 1680°C, and preferably the temperature is maintained for 3 to 12 hours, then poured into a forming mold for cooling and forming, preferably cooled to 750°C to 1000°C, then placed in an annealing furnace for annealing treatment, preferably the annealing temperature is 400°C to 650°C, and the annealing time is preferably 10 to 48 hours; then cooled to room temperature in the furnace, and the base glass is obtained. Those skilled in the art can select the type and amount of the refining agent according to the requirements, without creative labor. Further, the refining agent can include but is not limited to one or more of sodium chloride, tin oxide, antimony oxide or arsenic oxide, and the refining agent can be added in an amount of 0wt% to 1wt% of the total amount of the raw materials.
[0219] In some embodiments of the present application, the heat treatment process of the substrate glass can comprise a nucleation treatment and / or a crystallization treatment, preferably both a nucleation treatment and a crystallization treatment. In some embodiments, the crystallization treatment comprises a one-step crystallization treatment or a two-step crystallization treatment. In some embodiments, a two-step crystallization treatment can be used for preparing a curved glass-ceramic, and when a two-step crystallization treatment is used, the second step of the crystallization treatment is to place the crystallized glass material obtained from the first step of the crystallization treatment into a hot bending mold, heat to the crystallization temperature and perform a 3D hot bending forming process.
[0220] In some embodiments of the present application, in order to obtain the desired physical and chemical properties of the glass-ceramic, the heat treatment of the substrate glass can be performed in one step or in two or more steps. If the heat treatment is performed in one step, it means that the nucleation treatment (i.e., the nucleation treatment) is not performed separately, but a one-step heating is directly performed, and the nucleation and the growth of the target crystal are performed at the temperature reached in the one-step heating process, which can be understood as directly performing the crystallization treatment. If the heat treatment is performed in two steps, it means that a two-step heating process is performed, and the nucleation treatment (i.e., the nucleation treatment) is performed first, and then the growth of the target crystal (i.e., the crystallization treatment) is performed.
[0221] In some embodiments, in order to obtain the desired crystalline phase of the glass-ceramic and the desired physical and chemical properties, the temperature of the nucleation treatment can be 530-600°C, the time of the nucleation treatment can be 0-24h, preferably 2-8h; the temperature of the crystallization treatment can be 700-750°C, and the time of the crystallization treatment can be 0.10-24h, preferably 1-3h. When performing the heat treatment, the heating rate is preferably controlled to be 5-15°C / min, and more preferably the heating rate is 10°C / min. The temperature of the nucleation treatment refers to the temperature at which the crystal nucleus can form. The temperature of the crystallization treatment refers to the temperature at which the target crystal can grow controllably.
[0222] After the heat treatment, the skilled person in the art can also perform other conventional steps to obtain a glass-ceramic sample that meets the required specifications or requirements, such as shaping treatment, cutting treatment (such as cutting using a multi-wire cutting machine), CNC machining treatment (computer numerical control), thinning treatment or polishing treatment, etc.
[0223] In some embodiments of the present application, the chemical strengthening glass-ceramic with desired properties can be prepared by performing a specific chemical strengthening treatment on the aforementioned glass-ceramic.
[0224] In the present application, the chemical strengthening treatment, i.e. ion exchange method, is to immerse the glass-ceramics in a molten salt bath to exchange the alkali metal ions with smaller ionic radius in the glass-ceramics with the alkali metal ions with larger ionic radius in the molten salt bath, thereby forming a compressive stress layer on the surface of the glass-ceramics to obtain the glass-ceramics with better mechanical properties.
[0225] In some embodiments of the present application, the chemical strengthening treatment can be a single-step strengthening method or a multi-step strengthening method. The molten salt bath used in the chemical strengthening treatment is a molten salt bath containing sodium salt and / or potassium salt. Preferably, the molten salt bath used in the chemical strengthening treatment of the present application is a mixed molten salt bath containing sodium salt and potassium salt, and the temperature of the molten salt bath is preferably 380-500°C, more preferably 380-470°C. In some embodiments of the present application, the concentration of potassium salt in the salt bath is preferably 0-90wt%, and the concentration of sodium salt is 10-100wt%, more preferably a certain amount (e.g. 0-0.5wt%) of lithium salt is added to the salt bath. In some embodiments of the present application, the concentration of potassium salt in the salt bath is preferably 20-90wt%, and the concentration of sodium salt is 10-80wt%, more preferably 0.1-0.5wt% of lithium salt is added to the salt bath. In some embodiments of the present application, the time for the chemical strengthening treatment is preferably 0.1-6h, preferably 0.1-3h. The sodium salt can be selected from at least one of sodium nitrate, sodium sulfate and sodium carbonate, preferably sodium nitrate; the potassium salt can be selected from at least one of potassium nitrate, potassium sulfate and potassium carbonate, preferably potassium nitrate; and the lithium salt can be selected from at least one of lithium nitrate, lithium sulfate and lithium carbonate, preferably lithium nitrate.
[0226] The glass-ceramics or chemically strengthened glass-ceramics provided by the present application have excellent properties and can be used in electronic devices, including but not limited to mobile phones, tablet computers, handheld game consoles, portable digital devices (e.g. digital cameras), vehicle center control, electronic whiteboard glass, smart home, smart wear (e.g. smart bracelet, smart watch, smart glasses), vehicles, aircraft or vessels, and any desired glass-ceramic glassware. For example, it can be used in the display screen, cover glass, touch screen, inner screen or inner frame of an electronic device; for example, it can be used in the windshield, such as the front windshield or side windshield, of a vehicle, aircraft or vessel. For example, it can be used in a workbench, other surfaces, appliance doors, floor tiles, wall panels or storage containers. Other surfaces can include but are not limited to exterior wall surfaces, stair tread surfaces, column facings or counter surfaces, and storage containers can include but are not limited to cups, plates, medicine bottles or beverage bottles.
[0227] Exemplarily, the microcrystalline glass or chemically strengthened microcrystalline glass with excellent performance provided by the present application can be used to manufacture glass devices. The glass devices referred to herein can be regular or irregular, and can be manufactured according to requirements by those skilled in the art.
[0228] Exemplarily, the microcrystalline glass or chemically strengthened microcrystalline glass with excellent performance provided by the present application can be used to manufacture cover glass, which can be a display screen cover, a back cover or a camera protection cover of an electronic device. Exemplarily, the microcrystalline glass or chemically strengthened microcrystalline glass with excellent performance provided by the present application can be used in an electronic device. Referring to FIGS. 4, 5 and 6, in some embodiments of the present application, an electronic device, which can be a mobile phone, a tablet computer, a smart wearable device or the like, comprises a housing 1 assembled on the outer side of the electronic device, the housing 1 comprising a display screen cover 11 assembled on the front side and a back cover 12 assembled on the back side, the display screen cover 11 being covered on a display module 4, wherein the display screen cover 11 and / or the back cover 12 are made of the aforementioned microcrystalline glass or chemically strengthened microcrystalline glass. In the present application, the display screen cover 11 and the back cover 12 can be made of the aforementioned microcrystalline glass or chemically strengthened microcrystalline glass entirely or partially. In the present application, the display screen can be a touch display screen, and the display screen cover 11 can be a protection cover provided on the touch display screen. In the present application, the back cover 12 can cover only the back side (and the side away from the display screen) of the electronic device, or can cover the back side and the side frame of the electronic device, and optionally, the back cover 12 can cover all the side frames of the electronic device or can cover part of the side frames.
[0229] In some embodiments of the present application, as shown in FIG. 5, the electronic device further comprises a camera assembly 2 located inside the housing 1, and the housing 1 can comprise a camera protection cover 13, which is covered on the camera assembly 2 for protecting the camera assembly 2, and the camera protection cover 13 can be made of the aforementioned microcrystalline glass or chemically strengthened microcrystalline glass. In the present application, the camera protection cover 13 can be made of the aforementioned microcrystalline glass or chemically strengthened microcrystalline glass partially or entirely. In the present application, the camera protection cover 13 can be located on the front side of the electronic device or on the back side of the electronic device according to the location of the camera assembly 2. In some embodiments of the present application, the camera protection cover 13 can be in a separate structure from the display screen cover 11 or the back cover 12. In another embodiments of the present application, the camera protection cover 13 can be in an integrated structure with the display screen cover 11 or the back cover 12.
[0230] In some embodiments of the present application, as shown in FIG. 6, the electronic device further comprises a middle frame 3 between the display module 4 and the shell 1, and the middle frame 3 can comprise the aforementioned microcrystalline glass or chemically strengthened microcrystalline glass.
[0231] In the embodiments of the present application, the display screen cover plate, the back cover, the camera protection cover plate, and the middle frame in the electronic device can be any one of the four using the aforementioned microcrystalline glass or chemically strengthened microcrystalline glass, or any two of them using the aforementioned microcrystalline glass or chemically strengthened microcrystalline glass, or all three of them using the aforementioned microcrystalline glass or chemically strengthened microcrystalline glass, or all four of them using the aforementioned microcrystalline glass or chemically strengthened microcrystalline glass.
[0232] The technical solutions of the present application are further described in detail below in combination with embodiments. The embodiments of the present application described in detail below are exemplary and are only used to explain the present application and cannot be understood as a limitation of the present application.
[0233] Embodiment 1
[0234] (1) Preparation of base glass:
[0235] The raw materials (industrial conventional raw materials) were prepared according to the proportions of each component in Table 1, the total mass of the prepared raw materials was 1000g, 5g of clarifying agent sodium chloride (NaCl) was added to the prepared raw materials, and then the V-type mixer was mixed for 30 minutes to obtain a uniformly mixed raw material mixture.
[0236] The raw material mixture was transferred to a platinum crucible, then melted in the platinum crucible at 1650℃ for 5 hours, then poured into a forming mold for cooling, cooled to 900℃, then placed in a 500℃ annealing furnace for annealing for 24 hours, then cooled to room temperature with the furnace, and the base glass brick was obtained.
[0237] (2) Preparation of microcrystalline glass: According to the heat treatment process in Table 2, the base glass brick was placed in an annealing furnace, heated from room temperature to 550℃ at a rate of 10℃ / min for nucleation treatment, then heated to 710℃ at a rate of 10℃ / min for crystallization treatment, and then cooled to room temperature at a rate of 1℃ / min. The microcrystalline glass sample brick was obtained. The composition of the prepared microcrystalline glass is the same as that of the base glass, and the details are shown in Table 1.
[0238] The obtained glass-ceramic sample bricks are subjected to cold processing of cutting, CNC machining (the CNC instrument used in the present application is of RCG500S type), and polishing in sequence, and a glass-ceramic sample meeting the required specifications and requirements can be prepared. In Examples 1-7 and Comparative Examples 1-6 of the present application, the glass-ceramic sample bricks are subjected to the aforementioned cold processing to prepare glass-ceramic samples with a thickness of 0.70 mm, specifically, glass-ceramic polished sheet samples with a size of 50 mm x 50 mm x 0.70 mm or 157.79 mm x 73.82 mm x 0.70 mm.
[0239] Test conditions of the glass-ceramic sample obtained in Example 1:
[0240] The crystalline phase composition, crystallinity, average grain size, Vickers hardness, Young's modulus of the glass-ceramic sample, and the optical b value, haze, and transmittance (under 550 nm wavelength light) of the glass-ceramic sample with a thickness of 0.70 mm are tested respectively, and the results are shown in Table 2.
[0241] (3) Preparation of chemically strengthened glass-ceramic: the obtained glass-ceramic sample is placed in a strengthening furnace cavity and preheated for 5 min according to the chemical strengthening process in Table 3, and then quickly placed in a 460℃ molten salt bath for chemical strengthening treatment. The composition of the molten salt is 90wt% KNO3+10wt% NaNO3+0.15wt% LiNO3. Here, "0.15wt% LiNO3" means that 0.15wt% LiNO3 is added based on the total mass of KNO3 and NaNO3, and other similar expressions have similar meanings. After 3h of chemical strengthening treatment, the glass-ceramic sample is taken out and slowly cooled to room temperature on the furnace body of the strengthening furnace, and then the salt on the surface of the glass-ceramic is washed off with clean water. After drying the glass-ceramic sample, the chemically strengthened glass-ceramic is obtained.
[0242] Test conditions of the chemically strengthened glass-ceramic obtained in Example 1:
[0243] I. The DOL_0, CS_50, and |CT_AV| of the chemically strengthened glass-ceramic are measured under SLP-2000 stress instrument (the light source wavelength used is 518 nm, SOC=26 (nm / cm) / MPa, the refractive index is set to 1.56, and the exposure time is 300 μsec). The CT_LD value is calculated, and the results are shown in Table 3.
[0244] II. The surface Na2O mass percentage of the chemically strengthened glass-ceramic and the surface K2O mass percentage of the chemically strengthened glass-ceramic are measured by XRF, and the results are shown in Table 3. The values of formulas N and Y are calculated.
[0245] III. The average sandpaper drop height of the chemically strengthened glass-ceramics was tested, and the high temperature and high humidity test was performed on the chemically strengthened glass-ceramics, and the results are shown in Table 3.
[0246] Examples 2-7
[0247] Each of the examples was performed with reference to Example 1, except that the raw material composition of each example, different process parameters, and the corresponding test results thereof are shown in Tables 1-3.
[0248] The XRD pattern of the glass-ceramics of Example 1 is shown in FIG. 1, and it can be known from the figure that the main crystal phase in the glass-ceramics is lithium disilicate crystal phase.
[0249] The comparison chart of the transmittance curves of the glass-ceramics and the chemically strengthened glass-ceramics of Example 1 is shown in FIG. 2, and it can be known from the figure that the glass-ceramics and the chemically strengthened glass-ceramics prepared therefrom are both transparent in the visible light range, both have high transmittance, and the transmittance remains basically unchanged before and after chemical strengthening.
[0250] The comparison chart of the XRD patterns of the glass-ceramics and the chemically strengthened glass-ceramics of Example 1 is shown in FIG. 3, and it can be known from the figure that the crystal phase structure of the glass-ceramics does not change obviously before and after chemical strengthening, and the main crystal phase of the chemically strengthened glass-ceramics prepared from the glass-ceramics is also lithium disilicate crystal phase.
[0251] Comparative Examples 1-6
[0252] Each of the comparative examples was performed with reference to Example 1, except that the raw material composition of each comparative example, different process parameters, and the corresponding test results thereof are shown in Tables 1-3.
[0253] The physical comparison charts of the chemically strengthened glass-ceramics provided by Examples 1-3 and Comparative Examples 1-2 before and after the high temperature and high humidity test are shown in FIGS. 7-11, respectively, and in order to present the state of the chemically strengthened glass-ceramic sheet, the shooting was performed on the black background paper. It can be known from the comparison of the physical comparison charts that by meeting the specific relationship requirements between the mass percentages of Na2O and K2O on the surface of the chemically strengthened glass-ceramics and CT_LD, the application can ensure that the chemically strengthened glass-ceramics achieve better high temperature and high humidity resistance while ensuring that the chemically strengthened glass-ceramics meet the high stress level, indicating that the weather resistance is better.
[0254] Table 1
[0255] Note: The content percentage in molar of oxide in Table 1 is substituted into each formula, and the molar unit does not participate in the calculation of the formula.
[0256] Table 2
[0257] Table 3
[0258] From the above examples and comparative examples of Table 1-Table 3, for the same microcrystalline glass, by making the chemical strengthening microcrystalline glass meet the requirements of the relationship formula N of the present application, i.e., by making the surface Na2O mass percentage of the chemical strengthening microcrystalline glass, the surface K2O mass percentage of the chemical strengthening microcrystalline glass and the CT_LD satisfy a specific relationship, the chemical strengthening microcrystalline glass can have excellent stress level and excellent high temperature and high humidity resistance, and the obtained chemical strengthening microcrystalline glass can have higher mechanical strength performance and good weather resistance.
[0259] In the schemes of Comparative Example 1-Comparative Example 6, the surface Na2O mass percentage of the chemical strengthening microcrystalline glass and the surface K2O mass percentage of the chemical strengthening microcrystalline glass and the CT_LD do not satisfy the specific relationship, and finally, the prepared chemical strengthening microcrystalline glass either has spots or whitening marks that cannot be wiped off in the high temperature and high humidity test, and the weather resistance obviously does not meet the application requirements, or the stress level is low and the anti-drop damage performance is poor.
[0260] The above is only a specific embodiment of the present application and is not used to limit the present application. For those skilled in the art, the present application can have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application. Industrial applicability
[0261] The present application makes the surface composition and stress structure of the chemical strengthening microcrystalline glass with lithium disilicate as the main crystal phase satisfy a specific relationship, so that the chemical strengthening microcrystalline glass can achieve good weather resistance while meeting the high stress level, and can better guarantee that the chemical strengthening microcrystalline glass meets the market application requirements.
Claims
1. A chemically strengthened microcrystalline glass characterized in that, The chemical strengthening microcrystalline glass comprises lithium disilicate crystal phase, wherein the lithium disilicate crystal phase has a larger mass percentage than other crystal phases present in the chemical strengthening microcrystalline glass; the chemical strengthening microcrystalline glass has a compressive stress layer on the surface and a tensile stress in the interior; the chemical strengthening microcrystalline glass satisfies: N = n * (CT_LD-50000) / 10000, -32.5 < N < 15, preferably, -28.0 ≤ N ≤ 0, more preferably, -20.0 ≤ N ≤ -2.5, Wherein, n = (the mass percentage of Na2O on the surface of the chemically strengthened glass-ceramics / the mass percentage of K2O on the surface of the chemically strengthened glass-ceramics) 2 The mass percentage of Na2O on the surface of the chemically strengthened glass-ceramics and the mass percentage of K2O on the surface of the chemically strengthened glass-ceramics are determined by XRF; CT_LD is the linear density of tensile stress, in units of MPa / mm, and the data are substituted into the formula N according to the above unit requirements to obtain the calculation result, and the unit does not participate in the calculation.
2. The chemically strengthened glass-ceramic according to claim 1, wherein The chemical strengthening microcrystalline glass satisfies: 45000 MPa / mm ≤ CT_LD ≤ 52000 MPa / mm, preferably, 45900 MPa / mm ≤ CT_LD ≤ 50000 MPa / mm, more preferably, 47500 MPa / mm ≤ CT_LD ≤ 50000 MPa / mm.
3. The chemically strengthened glass-ceramics according to claim 1 or 2, characterized in that, The value of the formula N is -2.52, -4.07, -4.47, -4.75, -10.59, -11.90 or -12.73; and / or The value of CT_LD is 47517.24 MPa / mm, 48185.39 MPa / mm, 49692.43 MPa / mm, 47636.26 MPa / mm, 47919.69 MPa / mm, 47679.19 MPa / mm or 48097.14 MPa / mm.
4. The chemically strengthened glass ceramic according to any one of claims 1 to 3, wherein The surface Na2O mass percentage of the chemical strengthening microcrystalline glass is 5% to 8.5% by XRF determination in terms of mass percentage of oxide, preferably 5.5% to 7.5%; and / or, The surface K2O mass percentage of the chemical strengthening microcrystalline glass is 0.7% to 2.0% by XRF determination in terms of mass percentage of oxide, preferably 0.7% to 1.5%; and / or, The mass percentage of Na2O in the composition at the center of the chemical strengthening microcrystalline glass or the tensile stress layer is 3% to 3.5% in terms of mass percentage of oxide, preferably the mass percentage of Na2O is 3.1% to 3.2%.
5. The chemically strengthened glass ceramic according to any one of claims 1 to 4, wherein The surface Na2O mass percentage of the chemical strengthening microcrystalline glass is 5.30%, 6.12%, 7.00%, 5.21%, 6.32%, 5.17% or 6.36% by XRF determination in terms of mass percentage of oxide; and / or, The surface K2O mass percentage of the chemical strengthening microcrystalline glass is 1.25%, 0.81%, 0.77%, 1.24%, 0.80% or 1.26% by XRF determination in terms of mass percentage of oxide; and / or, The mass percentage of Na2O in the composition at the center of the chemical strengthening microcrystalline glass or the tensile stress layer is 3.16% or 3.14% in terms of mass percentage of oxide.
6. The chemically strengthened glass ceramic according to any one of claims 1 to 5, wherein, The chemical strengthening microcrystalline glass satisfies: Y = ΔC x ((CT_LD - 50000) / 100) 2 Y < 60, preferably Y < 50, more preferably Y < 20, wherein, ΔC is the difference between the mass percentage of Na2O at the surface of the chemically strengthened glass-ceramics and the mass percentage of Na2O at the center of the chemically strengthened glass-ceramics, the mass percentage of Na2O at the surface of the chemically strengthened glass-ceramics is determined by XRF; CT_LD is the tensile stress linear density, the unit is MPa / mm, the formula Y is calculated by substituting the data into the formula Y according to the above unit requirements, and the calculation result is obtained, and the unit is not involved in the calculation.
7. The chemically strengthened glass ceramic according to any one of claims 1 to 6, wherein, The value of formula Y is 0.36, 10.14, 11.58, 11.88, 13.02, 13.25 or 14.
84.
8. The chemically strengthened glass ceramic according to any one of claims 1 to 7, wherein, The chemically strengthened glass-ceramics satisfy: 75MPa≤|CT_AV|≤120MPa, preferably 77MPa≤|CT_AV|≤90MPa, wherein |CT_AV| is the absolute value of the average tensile stress; and / or, DOL_0 is 0.18t-0.25t, preferably 0.20t-0.25t, wherein DOL_0 is the depth of the compressive stress layer, and t is the thickness of the chemically strengthened glass-ceramics; and / or CS_50 is 150MPa-250MPa, preferably 160MPa-180MPa, wherein CS_50 refers to the compressive stress value at a depth of 50μm from the main surface of the chemically strengthened glass-ceramics.
9. The chemically strengthened glass ceramic according to any one of claims 1 to 8, wherein, The composition at the center or the tensile stress layer of the chemically strengthened glass-ceramics comprises, in terms of mole percentage of oxides: SiO2: 61.50%-63.40%, Al2O3: 2.75%-2.99%, P2O5: 0.91%-1.91%, ZrO2: 4.20%-4.85%, Na2O: 1.80%-3.20%, B2O3: 0-1.00%, and Li2O: 25.32%-26.52%.
10. The chemically strengthened glass ceramic according to any one of claims 1 to 9, wherein, The composition at the center or the tensile stress layer of the chemically strengthened glass-ceramics comprises, in terms of mole percentage of oxides: The mole percentage of SiO2 is 61.50%-63.30%, preferably the mole percentage of SiO2 is 62.00%-62.60%; and / or, The mole percentage of P2O5 is 1.20%-1.91%, preferably the mole percentage of P2O5 is 1.30%-1.60%; and / or, The mole percentage of Na2O is 1.85%-3.05%, preferably the mole percentage of Na2O is 2.20%-3.00%; and / or, The mole percentage of B2O3 is 0-0.65%; and / or, the mole percentage of ZrO2 is 4.20%-4.60%; and / or, The mole percentage of Li2O is 25.52%-26.52%, preferably the mole percentage of Li2O is 25.52%-26.00%.
11. The chemically strengthened glass ceramic according to any one of claims 1 to 10, wherein, The composition at the center or the tensile stress layer of the chemically strengthened glass-ceramics comprises, in terms of mole percentage of oxides: The mole percentage of SiO2 is 63.26%, 62.35% or 62.52%; and / or, The mole percentage of Al2O3 is 2.87%, 2.94% or 2.92%; and / or, The mole percentage of P2O5 is 1.20%-1.91%, preferably the mole percentage of P2O5 is 1.30%-1.60%; and / or, the molar percentage of P2O5 is 1.41% or 1.53%; and / or, the molar percentage of ZrO2 is 4.33% or 4.34%; and / or, the molar percentage of Na2O is 2.36%, 2.93% or 2.96%; and / or, the molar percentage of Li2O is 25.77%, 25.91% or 25.73%.
12. The chemically strengthened glass ceramic according to any one of claims 1 to 11, wherein, in the composition of the center or the tensile stress layer of the chemically strengthened glass-ceramics, the molar percentage of Na2O [Na2O], the molar percentage of B2O3 [B2O3] and the molar percentage of ZrO2 [ZrO2] satisfy the following relationship: Z = -1.344 x (2.65-100 x [Na2O])2+ 0.466 x 100 x [B2O3] + 1.203 x 100 x [ZrO2], 4.80≤Z≤5.35, preferably, 5.05≤Z≤5.25; and / or, in the composition of the center or the tensile stress layer of the chemically strengthened glass-ceramics, the molar percentage of Na2O [Na2O] and the molar percentage of B2O3 [B2O3] satisfy the following relationship: 0.90%≤[Na2O]-[B2O3]≤3.10%, preferably, 2.00%≤[Na2O]-[B2O3]≤3.00%, more preferably, 2.30%≤[Na2O]-[B2O3]≤3.00%; and / or, in the composition of the center or the tensile stress layer of the chemically strengthened glass-ceramics, the molar percentage of Na2O [Na2O] and the molar percentage of Li2O [Li2O] satisfy the following relationship: 8.55≤[Li2O] / [Na2O]≤13.85, preferably, 8.60≤[Li2O] / [Na2O]≤11.
00.
13. The chemically strengthened glass ceramic according to claim 12, wherein, the composition of the center or the tensile stress layer of the chemically strengthened glass-ceramics satisfies: the value of Z is 5.10, 5.09 or 5.12; and / or, the value of [Na2O]-[B2O3] is 2.36%, 2.93% or 2.96%; and / or, the value of [Li2O] / [Na2O] is 10.92, 8.84 or 8.
69.
14. The chemically strengthened glass ceramic of any one of claims 1 to 13, wherein, the mass of the lithium disilicate crystal phase accounts for more than 70% of all crystal phases of the chemically strengthened glass-ceramics, preferably, the mass of the lithium disilicate crystal phase accounts for more than 85% of all crystal phases of the chemically strengthened glass-ceramics.
15. The chemically strengthened glass ceramic of any one of claims 1 to 14, wherein, the average grain size of the chemically strengthened glass-ceramics is 40 nm or less, preferably, the average grain size is 15 nm to 35 nm; and / or, the crystallinity of the chemically strengthened glass-ceramics is 45% or more; preferably, the crystallinity of the chemically strengthened glass-ceramics is 45% to 85%, more preferably, the crystallinity of the chemically strengthened glass-ceramics is 55% to 65%.
16. The chemically strengthened glass ceramic of any one of claims 1 to 15, wherein, the chemically strengthened glass-ceramics is transparent in the visible light wavelength range, preferably, the transmittance of the chemically strengthened glass-ceramics is ≥ 90.00% for 550 nm wavelength light, preferably, the transmittance is > 90.40% at a thickness of 0.70 mm; and / or, The chemical strengthened glass-ceramics has a haze of <0.30% at a thickness of 0.70 mm, preferably a haze of <0.20%, and / or The chemical strengthened glass-ceramics has a b value of <0.70 at a thickness of 0.70 mm, preferably a b value of <0.
60.
17. The chemically strengthened glass ceramic of any one of claims 1 to 16, wherein, The chemical strengthened glass-ceramics has a Young's modulus of >100 GPa, preferably a Young's modulus of 105 GPa to 112.50 GPa; and / or The Vickers hardness of the chemically strengthened glass-ceramics is ≥ 650 kgf / mm 2 , preferably, the Vickers hardness of the chemically strengthened glass-ceramics is 650 kgf / mm 2 ~ 800 kgf / mm 2 .
18. The chemically strengthened glass ceramic of any one of claims 1 to 17, wherein, The chemical strengthened glass-ceramics is flat or curved; and / or, the chemical strengthened glass-ceramics has a thickness of 0.3 mm to 2 mm, preferably 0.45 mm to 0.8 mm; and / or, the chemical strengthened glass-ceramics does not contain a petalite crystal phase.
19. The chemically strengthened glass ceramic of any one of claims 1 to 18, wherein, The chemical strengthened glass-ceramics has a high temperature and high humidity failure time of >240 h at a temperature of 85°C and a relative humidity of 85%, wherein the high temperature and high humidity failure time is the total time from the start of the high temperature and high humidity test to the appearance of spots or whitening marks on the chemical strengthened glass-ceramics that cannot be wiped off.
20. A cover glass, characterized by The cover glass is made of or comprises the chemical strengthened glass-ceramics according to any one of claims 1 to 19.
21. An electronic device, comprising: The electronic device comprises the chemical strengthened glass-ceramics according to any one of claims 1 to 19.
22. The electronic device of claim 21, wherein, The electronic device comprises a housing assembled on the outer side of the electronic device, wherein the housing comprises the chemical strengthened glass-ceramics according to any one of claims 1 to 19.
23. The electronic device of claim 22, wherein, The housing comprises a display screen cover plate assembled on the front side of the electronic device, wherein the display screen cover plate comprises the chemical strengthened glass-ceramics according to any one of claims 1 to 19.
24. The electronic device of claim 22 or 23, wherein, The housing comprises a rear cover assembled on the rear side of the electronic device, wherein the rear cover comprises the chemical strengthened glass-ceramics according to any one of claims 1 to 19.
25. The electronic device of any of claims 22-24, wherein, The electronic device further comprises a camera assembly located inside the housing, wherein the housing comprises a camera protection cover plate covering the camera assembly, and the camera protection cover plate comprises the chemical strengthened glass-ceramics according to any one of claims 1 to 19.
26. The electronic device of any of claims 22-25, wherein, The electronic device further comprises a middle frame, wherein the middle frame comprises the chemical strengthened glass-ceramics according to any one of claims 1 to 19.
27. A glass article, characterized by, The glass device comprises the chemical strengthened glass-ceramics according to any one of claims 1 to 19.