120ksi-steel-grade high-strength high-toughness high-hydrogen sulfide-resistance hot-rolled steel round bar used for drill pipe joint, and preparation method therefor

MYUI2024006160UUndetermined Publication Date: 2023-10-29NANJING IRON & STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYUI2024006160
Authority / Receiving Office
MY · MY
Patent Type
Utility models
Current Assignee / Owner
Priority Date
2022-04-29
Filing Date
2022-07-12
Publication Date
2023-10-29
Estimated Expiration
2042-07-12

AI Technical Summary

Technical Problem

Existing low-alloy steel drilling rigs are prone to H2S stress corrosion cracking in high H2S environments, resulting in brittle fracture accidents in drilling materials and metal components far below the yield strength, which cannot meet the development needs of highly acidic gas fields.

Method used

Using 120ksi steel grade high strength, high toughness and advanced sulfur-resistant drill pipe joint hot-rolled round steel, it undergoes electric furnace smelting, LF refining, VD vacuum degassing, bloom high-precision continuous casting, billet inspection, heating furnace temperature control heating, rough rolling and Finish rolling and other processes control the chemical composition and structural uniformity to achieve high strength, toughness and hydrogen sulfide stress corrosion resistance.

Benefits of technology

It achieves high strength, toughness and resistance to hydrogen sulfide stress corrosion of drill pipe joints in high H2S environments. It is suitable for the development of sour oil and gas fields, significantly improves economic benefits, and is widely used in sour oil and gas fields and ultra-deep well production at home and abroad.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

Disclosed in the present invention are a 120ksi-steel-grade high-strength high-toughness high-hydrogen sulfide-resistance hot-rolled steel round bar used for a drill pipe joint, and a preparation method therefor. The chemical components of said steel comprise, by mass, 0.20-0.30% of C, 0.15-0.35% of Si, 0.45-0.75% of Mn, 1.10-1.50% of Cr, 0.60-0.80% of Mo, 0.020-0.060% of Nb, ≤0.008% of P, and ≤0.003% of S, with balances being Fe and inevitable impurities. The preparation method comprises: electric furnace, LF refining, vacuum degassing (VD), high-precision continuous casting, steel billet inspection, heating furnace temperature controlled heating, rough rolling, horizontal and vertical alternating high-precision continuous rolling, collection on a cooling bed, and finished product inspection. The hot-rolled steel round bar for a drill pipe joint has high strength, high toughness and strong hydrogen sulfide stress corrosion resistance and can be used for development of acidic oil and gas fields.
Need to check novelty before this filing date? Find Prior Art

Description

A 120ksi steel grade high-strength, high-toughness, high-grade sulfur-resistant hot-rolled round steel for drill pipe joints and its preparation method Technical Field

[0001] The invention relates to a hot-rolled round steel for a sulfur-resistant drill pipe joint and a preparation method thereof, and in particular to a 120ksi steel grade high-strength and high-toughness high-grade sulfur-resistant drill pipe joint and a preparation method thereof. Background Art

[0002] With the gradual development of my country's highly sour gas fields and advances in drilling technology, the demand for corrosion-resistant steel for drilling tools is increasing. Although my country possesses abundant oil and natural gas reserves, these resources contain high levels of H2S. For example, the Tarim Oil and Gas Field reports H2S concentrations as high as 12%, with even higher levels found in the North China Oilfield. Most of these oil and gas wells are deep and ultra-deep. Conventional low-alloy steel drilling and metal components used in such environments are susceptible to H2S stress corrosion cracking, leading to sudden brittle fracture of drill materials and metal components at temperatures far below their yield strength. Therefore, developing new steel grades with higher H2S stress corrosion resistance is a pressing issue for energy development and the full utilization of oil and gas resources. Developing high-grade H2S stress corrosion-resistant steel not only offers significant socioeconomic benefits but also holds promising market prospects.

[0003] 120ksi steel grade high strength and high toughness hot-rolled round steel for drill pipe joints resistant to hydrogen sulfide stress corrosion cracking is a high-tech variety. The control of inclusions, ultra-low P and S smelting, and the control of round steel structure uniformity are issues that need to be addressed by technical personnel in this field.

[0004] Summary of the Invention

[0005] Purpose of the invention: The present invention aims to provide a 120ksi steel grade high-strength, high-toughness, high-grade sulfur-resistant drill pipe joint hot-rolled round steel with high strength, high toughness, good resistance to hydrogen sulfide stress corrosion, suitable for the development of sour oil and gas fields, and stable performance; another object of the present invention is to provide a method for preparing 120ksi steel grade high-strength, high-toughness, high-grade sulfur-resistant drill pipe joint hot-rolled round steel.

[0006] Technical solution: The 120ksi steel-grade high-strength, high-toughness, and high-grade sulfur-resistant hot-rolled round steel for drill pipe joints of the present invention has the following chemical compositions by mass percentage: C 0.20%-0.30%, Si 0.15%-0.35%, Mn 0.45%-0.75%, Cr 1.10%-1.50%, Mo 0.60%-0.80%, Nb 0.020%-0.060%, P≤0.008%, S≤0.003%, and the balance being Fe and unavoidable impurities.

[0007] The method for preparing 120ksi steel-grade high-strength, high-toughness, and high-grade sulfur-resistant hot-rolled round steel for drill pipe joints includes electric furnace smelting, LF refining, VD vacuum degassing, large square bloom high-precision continuous casting, billet inspection, heating in a heating furnace with temperature control, rough rolling, horizontal and vertical alternating high-precision continuous rolling, long cooling bed collection, and finished product inspection. The steps are as follows:

[0008] The molten steel is smelted in an electric furnace, with active lime added into the furnace and oxygen supplied. The oxygen level of the tapped steel is guaranteed to be ≤200ppm, the C content is 0.06%, and the P content of the tapped steel is within 0.008%. Molybdenum-iron alloy, high-carbon ferroalloy, etc. are added to alloy the molten steel.

[0009] The molten steel smelted in the electric furnace is tapped through the eccentric bottom of the furnace and refined in an LF refining furnace, and aluminum wire and high-purity silicon carbide are added to the LF refining furnace for deoxidation; the composition is controlled to be C 0.20%-0.30%, Si 0.15%-0.35%, Mn 0.45%-0.75%, Cr 1.10%-1.50%, Mo 0.60%-0.80%, Nb 0.020%-0.060%, P ≤ 0.008%, and S ≤ 0.003%;

[0010] After the molten steel composition and temperature are qualified, the ladle furnace is hoisted to the VD vacuum degassing treatment station for vacuum treatment;

[0011] The molten steel after vacuum treatment is hoisted to the continuous casting station for casting. Electromagnetic stirring of the crystallizer and electromagnetic stirring of the end are used. The large rectangular billets cast have center segregation and center porosity within 1.0 level, and no defects such as shrinkage cavities and subcutaneous cracks.

[0012] The bloom is placed in a heating furnace and heated in a reducing atmosphere with the residual oxygen content in the flue gas below 3%. The starting rolling temperature, intermediate rolling inlet temperature, final rolling outlet temperature, and upper cooling bed temperature are set to 1060-1160°C, 950-1000°C, 850-900°C, and below 700°C, respectively. The heated bloom is descaled with high-pressure water and then sent to the rolling process. After rough rolling and finish rolling, the finished product is transported to the cooling bed via conveyor rollers and collected on the cooling bed after cooling.

[0013] The finished products after rolling are collected on a cooling bed for windproof cooling, and the surface quality and dimensional tolerance are checked. Then they are packaged, labeled, weighed, labeled, and put into storage to obtain 120ksi steel grade high-strength, high-toughness, and high-grade sulfur-resistant hot-rolled round steel for drill pipe joints.

[0014] Preferably, the oxygen supply during smelting molten steel in the electric furnace is 30-60m 3 / ton.

[0015] Preferably, the refining time is 35-120 min.

[0016] Preferably, the vacuum degree during the vacuum treatment is controlled within 1 mbar.

[0017] Preferably, the vacuum treatment is carried out for 12-30 minutes, and after breaking the vacuum, the Ar gas is soft-blown and stirred for 10-25 minutes.

[0018] Preferably, during the casting, the superheat is controlled to be 10° C.-50° C. and the pulling speed is 0.45-0.55 m / min.

[0019] Preferably, the heating section of the heating furnace is controlled at 1000-1280°C, and the soaking section is controlled at 1200-1280°C, to ensure that the temperature difference of the steel billet cross section is less than 30°C.

[0020] Preferably, in the rolling process, the number of rough rolling passes is 6-8 and the number of finishing rolling passes is 8-10.

[0021] Preferably, the temperature of the cooling bed is controlled to be lower than 500°C during collection.

[0022] Based on the production line characteristics and product properties, the present invention develops a composition design of a low-carbon Cr-Mo-Nb alloy system and designs the metallurgical composition of 120ksi steel grade high-strength, high-toughness, hydrogen sulfide stress corrosion cracking resistant hot-rolled round steel for drill pipe joints;

[0023] Through the study of hydrogen sulfide stress corrosion mechanism, the electric furnace ultra-low P and S smelting process and inclusion control are adopted to achieve P≤0.008%, S≤0.003% in steel, and the inclusion content of the whole system is less than 0.5 level;

[0024] Through the study of continuous casting billet drawing speed, electromagnetic stirring, and secondary cooling water cooling intensity, the homogenization control of the billet is achieved; the rolling process achieves uniform control of the hot-rolled round steel structure through rough and fine continuous rolling and slow cooling mechanisms.

[0025] Beneficial effects: Compared with the existing technology, the present invention has the following significant advantages: (1) It has high strength, high toughness, good resistance to hydrogen sulfide stress corrosion, and is suitable for the development of sour oil and gas fields; after the drill pipe joint undergoes a suitable heat treatment process, the product successfully passes the 720-hour performance test of resistance to hydrogen sulfide stress corrosion; (2) It has significant economic benefits. The product is widely used in sour oil and gas fields and ultra-deep well mining at home and abroad such as Tarim, and the social and economic benefits generated are immeasurable. DETAILED DESCRIPTION

[0026] The technical solution of the present invention will be further described below in conjunction with specific embodiments.

[0027] Example 1

[0028] A 120 ksi steel grade high-strength, high-toughness, high-grade sulfur-resistant hot-rolled round steel for drill pipe joints. The chemical composition is shown in Table 1.

[0029] The preparation method of 120ksi steel grade high-strength, high-toughness and high-grade sulfur-resistant hot-rolled round steel for drill pipe joints comprises the following steps: 100-ton electric furnace - 100-ton LF refining furnace - 100-ton VD vacuum furnace - 320mm×480mm small square billet continuous casting - billet inspection - temperature-controlled heating in a three-stage continuous pusher-type heating furnace - rolling in a Φ850 roughing mill - intermediate rolling - finishing rolling - collection on a cooling bed - inspection - windproof pile cooling - round steel bar - joint processing - quenching and tempering treatment.

[0030] (1) Smelting process

[0031] Molten steel is blown in a 100-ton electric furnace. After the furnace, alloys and composite aluminum are added for precipitation deoxidation and alloying. The tapped steel has a carbon content of 0.07% and a phosphorus content of 0.006%. Aluminum shot, high-purity graphite, and high-purity silicon carbide are added in small, multi-batch quantities. Refining takes 40-45 minutes. See Table 1 for details on composition control.

[0032] After the LF refining component temperature is qualified, VD vacuum degassing is carried out, the vacuum degree is 0.8mbar-2.5mbar, and the vacuum holding time is 12-30min. After breaking the vacuum, add a bag of covering agent and stir with soft Ar for 10min-25min. When stirring statically, the slag surface moves slightly and no light is seen.

[0033] The vacuum-treated molten steel is hoisted into a large square billet continuous casting machine for casting. Four streams are cast at an overheat of 25°C, a casting speed of 0.48m / min-0.57m / min, and electromagnetic stirring of the crystallizer and the end of the mold. Large square billets with a cross-section of 320mm×480mm are cast.

[0034] (2) Steel rolling process

[0035] A 320mm x 480mm billet was placed in a walking beam furnace and heated in a reducing atmosphere with a flue gas residual oxygen content of 2.1%. The heating section of the furnace was controlled at 1200°C, the soaking section at 1230°C, and the cross-sectional temperature difference of the billet was 25°C.

[0036] After being heated, the 320mm x 480mm square billets are descaled with high-pressure water and then sent to the rolling process, where they are rolled to a Φ110mm gauge. Rough rolling begins at 1100°C, and after six passes of rough rolling, intermediate and finishing rolling is performed. Intermediate rolling begins at 980°C, finishes at 900°C, and the upper cooling bed is 820°C. After rolling, the steel is slowly cooled and collected to produce high-grade, sulfur-resistant hot-rolled round steel.

[0037] (3) Product processing

[0038] The round steel is die-forged into a drill pipe joint, quenched and heated at 940±20℃ for 230±15 minutes in the furnace, cooled with quenching liquid, tempered and heated at 630±20℃ for 260±15 minutes in the furnace, and then cooled to room temperature after being taken out of the furnace to obtain a quenched and tempered joint.

[0039] Example 2

[0040] A 120 ksi steel grade high-strength, high-toughness, high-grade sulfur-resistant hot-rolled round steel for drill pipe joints, the chemical composition of which is shown in Table 1. The preparation method is the same as that of Example 1.

[0041] Example 3

[0042] A 120 ksi steel grade high strength, high toughness and high sulfur resistance hot rolled round steel for drill pipe joints, the chemical composition of which is shown in Table 1. The preparation method is the same as that of Example 1.

[0043] Example 4

[0044] A 120 ksi steel grade high-strength, high-toughness, high-grade sulfur-resistant hot-rolled round steel for drill pipe joints, the chemical composition of which is shown in Table 1. The preparation method is the same as that of Example 1.

[0045] Example 5

[0046] A 120 ksi steel grade high-strength, high-toughness, high-grade sulfur-resistant hot-rolled round steel for drill pipe joints, the chemical composition of which is shown in Table 1. The preparation method is the same as that of Example 1.

[0047] Comparative Example

[0048] Common 120ksi primary sulfur-resistant joint steel, its chemical composition is shown in Table 1.

[0049] Table 1 Chemical composition (wt%) (the balance is Fe and other inevitable impurities except P and S)

[0050] Element CSiMnPSCrMoNbV Example 1 0.27 0.25 0.60 0.005 0.001 1.35 0.68 0.040 / Example 2 0.30 0.22 0.75 0.007 0.003 1.16 0.80 0.060 / Example 3 0.22 0.28 0.56 0.005 0.002 1.45 0.60 0.020 / Example 4 0.25 0.30 0.47 0.008 0.001 1.48 0.78 0.035 / Example 5 0.20 0.35 0.68 0.004 0.002 1.23 0.75 0.039 / Comparative Example 0.25 0.23 1.00 0.006 0.002 1.10 0.60 0.03 0.06

[0051] Product mechanical properties testing: Comparison of the quenched and tempered joints in Examples 1-5 with the ordinary 120ksi primary sulfur-resistant joint steel of the same specification shows high strength, high low-temperature toughness, improved elongation after fracture and area reduction. See Table 2 below for detailed comparison.

[0052] Table 2 Comparison of mechanical properties between examples and comparative examples

[0053]

[0054] Product hydrogen sulfide resistance test: The A-NACE constant load tensile test method was used to test the material's sulfur resistance using solution A to simulate a hydrogen sulfide corrosion environment. The standard tensile specimen of the material showed no cracking after 720 hours, indicating excellent sulfur resistance. The results of the hydrogen sulfide stress corrosion resistance test are shown in Table 3.

[0055] Table 3 Hydrogen sulfide stress corrosion test results

[0056]

Claims

1. A 120ksi steel grade high strength, high toughness and high sulfur resistant hot rolled round steel for drill pipe joints, characterized in that: Its chemical composition, by mass percentage, includes: C 0.20%-0.30%, Si 0.15%-0.35%, Mn 0.45%-0.75%, Cr 1.10%-1.50%, Mo 0.60%-0.80%, Nb 0.020%-0.060%, P≤0.008%, S≤0.003%, and the balance is Fe and unavoidable impurities.

2. A method for preparing the 120ksi steel grade high-strength, high-toughness, high-grade sulfur-resistant hot-rolled round steel for drill pipe joints according to claim 1, characterized in that: It includes electric furnace smelting - LF refining - VD vacuum degassing - large square bloom high-precision continuous casting - billet inspection - heating furnace temperature control - rough rolling - horizontal and vertical alternating high-precision continuous rolling - long cooling bed collection - finished product inspection; the steps are as follows: The molten steel is smelted in an electric furnace, with active lime added into the furnace and oxygen supplied. The oxygen level of the tapped steel is guaranteed to be ≤200ppm, the C content is 0.06%, and the P content of the tapped steel is within 0.008%. Molybdenum-iron alloy, high-carbon ferroalloy, etc. are added to alloy the molten steel. The molten steel smelted in the electric furnace is tapped through the eccentric bottom of the furnace and refined in an LF refining furnace, and aluminum wire and high-purity silicon carbide are added to the LF refining furnace for deoxidation; the composition is controlled to be C 0.20%-0.30%, Si 0.15%-0.35%, Mn 0.45%-0.75%, Cr 1.10%-1.50%, Mo 0.60%-0.80%, Nb 0.020%-0.060%, P ≤ 0.008%, and S ≤ 0.003%; After the molten steel composition and temperature are qualified, the ladle furnace is hoisted to the VD vacuum degassing treatment station for vacuum treatment; The molten steel after vacuum treatment is hoisted to the continuous casting station for casting. Electromagnetic stirring of the crystallizer and electromagnetic stirring of the end are used. The large rectangular billets cast have center segregation and center porosity within 1.0 level, and no defects such as shrinkage cavities and subcutaneous cracks. The bloom is placed in a heating furnace and heated in a reducing atmosphere with the residual oxygen content in the flue gas below 3%. The starting rolling temperature, intermediate rolling inlet temperature, final rolling outlet temperature, and upper cooling bed temperature are set to 1060-1160°C, 950-1000°C, 850-900°C, and below 700°C, respectively. The heated bloom is descaled with high-pressure water and then sent to the rolling process. After rough rolling and finish rolling, the finished product is transported to the cooling bed via conveyor rollers and collected on the cooling bed after cooling. The finished products after rolling are collected on a cooling bed for windproof cooling, and the surface quality and dimensional tolerance are checked. Then they are packaged, labeled, weighed, labeled, and put into storage to obtain 120ksi steel grade high-strength, high-toughness, and high-grade sulfur-resistant hot-rolled round steel for drill pipe joints.

3. A method for preparing the 120ksi steel grade high strength, high toughness and high sulfur resistant hot rolled round steel for drill pipe joints according to claim 2, characterized in that: The oxygen supply during smelting molten steel in the electric furnace is 30-60m 3 / ton.

4. A method for preparing the 120ksi steel grade high strength, high toughness and high sulfur resistant hot rolled round steel for drill pipe joints according to claim 2, characterized in that: The refining time is 35-120 minutes.

5. A method for preparing the 120ksi steel grade high strength, high toughness and high sulfur resistant hot rolled round steel for drill pipe joints according to claim 2, characterized in that: The vacuum degree during the vacuum treatment is controlled within 1 mbar.

6. A method for preparing the 120ksi steel grade high strength, high toughness and high sulfur resistant hot rolled round steel for drill pipe joints according to claim 2, characterized in that: The vacuum treatment is performed with a vacuum holding time of 12 min to 30 min, and Ar gas is soft-blown and stirred for 10 min to 25 min after the vacuum is broken.

7. A method for preparing the 120ksi steel grade high strength, high toughness and high sulfur resistant hot rolled round steel for drill pipe joints according to claim 2, characterized in that: During the casting, the superheat is controlled to be 10° C.-50° C. and the pulling speed is 0.45-0.55 m / min.

8. A method for preparing the 120ksi steel grade high strength, high toughness and high sulfur resistant hot rolled round steel for drill pipe joints according to claim 2, characterized in that: The heating section of the heating furnace is controlled at 1000-1280°C, and the soaking section is controlled at 1200-1280°C, ensuring that the temperature difference of the steel billet cross section is less than 30°C.

9. A method for preparing the 120ksi steel grade high strength, high toughness and high sulfur resistant hot rolled round steel for drill pipe joints according to claim 2, characterized in that: In the rolling process, the rough rolling passes are 6-8 passes, and the finishing rolling passes are 8-10 passes.

10. A method for preparing the 120ksi steel grade high strength, high toughness and high sulfur resistant hot rolled round steel for drill pipe joints according to claim 2, characterized in that: The temperature of the cooling bed is controlled to be lower than 500° C. during collection.