Slurry design process
Patent Information
- Application Number
- NO20190823
- Authority / Receiving Office
- NO · NO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2017-02-22
- Filing Date
- 2019-06-28
- Publication Date
- 2019-06-28
- Estimated Expiration
- 2039-06-28
Abstract
Description
SLURRY DESIGN PROCESSBACKGROUND
[0001] In well cementing, such as well construction and remedial cementing, cement compositions are commonly utilized. Cement compositions may be used in a variety of subterranean applications. For example, in subterranean well construction, a pipe string (e.g., casing, liners, expandable tubulars, etc.) may be run into a well bore and cemented in place. The process of cementing the pipe string in place is commonly referred to as “primary cementing.” In a typical primary cementing method, a cement composition may be pumped into an annulus between the walls of the well bore and the exterior surface of the pipe string disposed therein. The cement composition may set in the annular space, thereby forming an annular sheath of hardened, substantially impermeable cement (i.e., a cement sheath) that may support and position the pipe string in the well bore and may bond the exterior surface of the pipe string to the subterranean formation. A mong other things, the cement sheath surrounding the pipe string functions to prevent the migration of fluids in the annulus, as well as protecting the pipe string from corrosion. Cement compositions also may be used in remedial cementing methods, for example, to seal cracks or holes in pipe strings or cement sheaths, to seal highly permeable formation zones or fractures, to place a cement plug, and the like.
[0002] A particular challenge in well cementing is the development of satisfactory mechanical properties in a cement composition within a reasonable time period after placement in the subterranean formation. Oftentimes several cement compositions with varying additives are tested to see if they meet the material engineering requirements for a particular well. The process of s electing the components of the cement composition are usually done by a best guess approach by utilizing previous slurries and modifying them until a satisfactory solution is reached. The process may be time consuming and the resulting slurry may be expensive. Furthermore, the cement components available in any one particular region may vary in composition from those of another region thereby further complicating the process of selecting a correct slurry.1BRIEF DESCRIPTION OF THE DRAWINGS
[0003] These drawings illustrate certain aspects of some of the embodiments of the present invention, and should not be used to limit or define the invention.
[0004] FIG. 1 is a chart showing simulated results for compressive strength index calculations.
[0005] FIG. 2 is a chart showing simulated results for compressive strength index calculations.
[0006] FIG. 3 is a schematic illustration of an example system for analyzing cement components.
[0007] FIG. 4 is a schematic illustration of an example system for generating cement compositions.
[0008] FIG. 5 is a schematic illustration of s howing introduction of a c ement composition into a wellbore.DETAILED DESCRIPTION
[0009] The present disclosure may generally relate to cementing methods and system. Provided herein are methods of i dentifying and categorizing silica sources, cements, and other materials based on physiochemical properties. The physiochemical properties of each cement component of a cement composition may affect the final set mechanical properties of the slurry as well as the dynamic or time based properties such as mixability, rheology, viscosity, and others. Every cement component may affect one or more of the properties mentioned, sometimes unpredictably. For example, a locally sourced fly ash may be added to a cement composition. The added fly ash may increase the compressive strength of the cement composition and may have no effect on for example, the thickening time of the cement composition. In another region, a locally sourced fly ash may also increase the compressive strength of the cement composition but may also increase the thickening time. The unpredictable behavior of a cement composition may not be realized until multiple lab tests have been performed.
[0010] The cement compositions generally may comprise water and a cement additive. The cement additive may comprise two or more cement components, which may be dry blended to form the cement additive prior to combination with the water. Alternatively, the cement components may not be combined until mixture with the water. The cement components may generally be described as alkali soluble. A cement composition may 2comprise water and a cement additive, wherein the cement additive comprises hydraulic cement, cement kiln dust, and a natural pozzolan. As described in more detail herein, the cement compositions may be foamed and / or extended as desired by those of ordinary skill in the art.
[0011] The cement compositions may have a density suitable for a particular application. The cement compositions may have a density in the range of about 8 pounds per gallon (“ppg”) to about 16 ppg. In the foamed examples, the foamed cement compositions of the present invention may have a density in the range of about 8 ppg to about 13 ppg (or even lower).
[0012] The water used in the cement compositions may include, for example, freshwater, saltwater (e.g., water containing one or more salts dissolved therein), brine (e.g., saturated saltwater produced from subterranean formations), seawater, or combinations thereof. Generally, the water may be from any source, provided that it does not contain an excess of c ompounds that may undesirably affect other components in the cementcomposition. The water may be included in an amount sufficient to form a pumpable slurry. The water may be included in the cement compositions in the range of about 40% to about 200% by weight of the cement additive (“bwoc”). In some examples, the water may be included in an amount in the range of about 40% to about 150% bwoc.
[0013] The cement additive may comprise two or more cement components. One of the cement components may comprise a hydraulic cement. A variety of hydraulic cements may be utilized in accordance with the present disclosure, including, but not limited to, those comprising calcium, aluminum, silicon, oxygen, iron, and / or sulfur, which set and harden by reaction with water. Suitable hydraulic cements may include Portland cements, gypsum, andhigh alumina content cements, among others. Portland cements that are suited for use in the present disclosure may be classified as Classes A, C, G, and H cements according to American Petroleum Institute, API Specification for Materials and Testing for Well Cements, API Specification 10, Fifth Ed., Jul. 1, 1990. In addition, in some examples, cements suitable for use in the present invention may be classified as ASTM Type I, II, or III. Cement compositions that may be considered “low Portland” may be designed by use of t he techniques disclosed herein.
[0014] Where present, the hydraulic cement generally may be included in the cement compositions in an amount sufficient to provide the desired compressive strength, density, and / or cost. The hydraulic cement may be present in the cement compositions in an amount in the range of about 0% to about 99% bwoc. In some examples the hydraulic cement may be 3present in an amount ranging between any of and / or including any of about 1%, about 5%, about 10%, about 20%, about 40%, about 60%, about 80%, or a bout 90% bwoc. The cement component may be considered “low Portland” in that the Portland cement (where used) may be present in the cement composition in an amount of a bout 40% or less bwoc and, alternatively, about 20% or less. The cement compositions may also be designed that are free (or essentially free) of Portland cement. Those of ordinary skill in the art, with the benefit of this disclosure, should be able to select an appropriate amount of hydraulic cement for a particular application.
[0015] In addition to hydraulic cement, additional cement components may be used that can be considered alkali soluble. A cement component is considered alkali soluble where it is at least partially soluble in an aqueous solution of pH 7.0 or greater. Certain of the alkali soluble cement components may comprise a geopolymer cement, which may comprise an aluminosilicate source, a metal silicate source, and an activator. The geopolymer cement may react to form a geopolymer. A geopolymer is an inorganic polymer that forms long-range, covalently bonded, non-crystalline networks. Geopolymers may be formed by chemical dissolution and subsequent re-condensation of various aluminosilicates and silicates to form a 3D-network or three-dimensional mineral polymer.
[0016] The activator for the geopolymer cement may include, but is not limited to, metal hydroxides chloride salts such as KCl, CaCl , NaCl, carbonates such as Na CO , 2 2 3silicates such as sodium silicate, aluminates such as sodium aluminate, and ammonium hydroxide.
[0017] The aluminosilicate source for the geopolymer cement may comprise any suitable aluminosilicate. Aluminosilicate is a mineral comprising aluminum, silicon, and oxygen, plus counter-cations. There are potentially hundreds of suitable minerals that may be an aluminosilicate source in that they m ay comprise aluminosilicate minerals. Each aluminosilicate source may potentially be used in a particular case if the specific properties, such as composition, may be known. Some minerals such as andalusite, kyanite, and sillimanite are naturally occurring aluminosilicate sources that have the same composition, Al SiO , but differ in crystal structure. Each mineral andalusite, kyanite, or sillimanite may 2 5react more or less quickly and to different extents at the same temperature and pressure due to the differing crystal structures. Other suitable aluminosilicate sources may include, but are not limited to, calcined clays, partially calcined clays, kaolinite clays, lateritic clays, illite clays, volcanic rocks, mine tailings, blast furnace slag, and coal fly ash.4
[0018] The metal s ilicate source for the geopolymer cement may comprise any suitable metal silicate. A silicate is a compound containing an anionic silicon compound. Some examples of a silicate include the orthosilicate anion also known as silicon tetroxide 4- 2-anion, SiO as well as hexafluorosilicate [SiF ] . Other common silicates include cyclic and 4 62n-single chain silicates which may have the general f ormula [SiO ] and sheet-forming 2+n-silicates ([SiO ] ) . Each silicate example may have one or more metal cations associated 2.5 nwith each silicate molecule. Some suitable metal silicate sources and may include, without limitation, sodium silicate, magnesium silicate, and potassium silicate.
[0019] Where present, the geopolymer cement generally may be included in the cement compositions in an amount sufficient to provide the desired compressive strength, density, and / or cost. The geopolymer cement may be present in the cement compositions in an amount in the range of about 0% to about 99% bwoc. In some examples the geopolymercement may be present in an amount ranging between any of and / or including any of about 1%, about 5%, about 10%, about 20%, about 40%, about 60%, about 80%, or about 90% bwoc. Those of ordinary skill in the art, with the benefit of this disclosure, should be able to select an appropriate amount of geopolymer cement for a particular application.
[0020] Additional cement components that are alkali soluble may be considered a silica source. By inclusion of the silica source, a different path may be used to arrive at a similar product as from Portland cement. A pozzolanic reaction may be induced wherein silicic acid (H SiO ) and portlandite (Ca(OH) react to form a cement product (calcium 4 4 2silicate hydrate). If other compounds, such as, aluminate, are present in the silica source, additional reactions may occur to form a dditional cement products, such as calcium aluminate hydrates. Calcium hydroxide necessary for the reaction may be provide from other cement components, such as Portland cement, or may be separately added to the cement composition. Examples of suitable silica sources may include fly ash, slag, silica fume, crystalline silica, silica flour, cement kiln dust (“CKD”), volcanic rock, perlite, metakaolin, diatomaceous earth, zeolite, shale, and agricultural waste ash (e.g., rice husk ash, sugar cane ash, and bagasse ash), among other. Some specific examples of the silica source will be discussed in more detail below. Where present, the silica source generally may be included in the cement compositions in an amount sufficient to provide the desired compressive strength, density, and / or cost. The silica source may be present in the cement compositions in an amount in the range of about 0% to about 99% bwoc. In some examples the silica source may be present in an amount ranging between any of and / or including any of about 1%, about 5%, about 10%, about 20%, about 40%, about 60%, about 80%, or about 90% bwoc. Those of 5ordinary skill in the art, with the benefit of this disclosure, should be able to select an appropriate amount of silica source for a particular application.
[0021] An example of a suitable silica source may comprise fly ash. A variety of fly ash may be suitable, including fly ash classified as Class C and Class F fly ash according to American Petroleum Institute, API Specification for Materials and Testing for Well Cements, API Specification 10, Fifth Ed., July 1, 1990. Class C fly ash comprises both silica and lime, so it may set to form a hardened mass upon mixing with water. Class F fly ash generally does not contain a sufficient amount of lime to induce a cementitious reaction, therefore, an additional source of calcium ions is necessary for a set-delayed cement composition comprising Class F fly ash. In some embodiments, lime may be mixed with Class F fly ash in an amount in the range of about 0.1% to about 100% by weight of the fly ash. In some instances, the lime may be hydrated lime. ®Suitable examples of fly a sh include, but are not limited to, POZMIX A cement additive, commercially available from Halliburton Energy Services, Inc., Houston, Texas.
[0022] Another example of a s uitable silica source may comprise slag. Slag is generally a by-product in the production of various metals from their corresponding ores. By way of example, the production of cast iron can produce slag as a granulated, blast furnace by-product with the slag generally comprising the oxidized impurities found in iron ore. Slag generally does not contain sufficient basic material, so slag cement may be used that further may comprise a base to produce a settable composition that may react with water to set to form a hardened mass. Examples of suitable sources of bases include, but are not limited to, sodium hydroxide, sodium bicarbonate, sodium carbonate, lime, and combinations thereof.
[0023] Another example of a suitable silica source may comprise CKD. Cement kiln dust or “CKD”, as that term is used herein, refers to a partially calcined kiln feed which is removed from the gas stream and collected, for example, in a dust collector during the manufacture of cement. Usually, large quantities of CKD are collected in the production of cement that are commonly disposed of as waste. Disposal of the CKD as waste can add undesirable costs to the manufacture of the cement, as well as the environmental concerns associated with its disposal. CKD is another component that may be included in examples of the cement compositions.
[0024] Another example of a suitable silica source may comprise volcanic rock. Certain volcanic rocks can exhibit cementitious properties, in that they may set and harden in the presence of hydrated lime and water. The volcanic rock may also be ground, for example. Generally, the volcanic rock may have any particle size distribution as desired for a particular application. In certain embodiments, the volcanic rock may have a mean particle 6size in a range of f rom about 1 micron to about 200 microns. The mean particle size corresponds to d50 values as measured by particle size analyzers such as those manufactured by Malvern Instruments, Worcestershire, United Kingdom. One of ordinary skill in the art, with the benefit of this disclosure, should be able to select a particle size for the volcanic rocksuitable for use for a chosen application.
[0025] Another example of a s uitable silica source may comprise metakaolin. Generally, metakaolin is a white pozzolan that may be prepared by heating kaolin clay, for example, to temperatures in the range of about 600° to about 800°C.
[0026] Another example of a suitable silica source may comprise shale. Among other things, shale included in the cement compositions may react with excess lime to form a suitable cementing material, for example, calcium silicate hydrate. A variety of shales are suitable, including those comprising silicon, aluminum, calcium, and / or magnesium. An example of a suitable shale comprises vitrified shale. Generally, the shale may have any particle size distribution as desired for a particular application. In certain embodiments, the shale may have a particle size distribution in the range of about 37 micrometers to about 4,750 micrometers.
[0027] Another example of a suitable silica source may comprise zeolite. Zeolites generally are porous alumino-silicate minerals that may be either a natural or synthetic material. Synthetic zeolites are based on the same type of structural cell as natural zeolites, and may comprise aluminosilicate hydrates. As used herein, the term “zeolite” refers to all natural and synthetic forms of zeolite. Examples of zeolites may include, without limitation, mordenite, zsm-5, zeolite x, zeolite y, z eolite a, etc. Furthermore, examples comprising + + 2+ 2+zeolite may comprise zeolite in combination with a cation such as Na , K , Ca , Mg , etc. Zeolites comprising cations such as sodium may also provide additional cation sources to the cement composition as the zeolites dissolve.
[0028] The cement compositions may further comprise hydrated lime. As used herein, the term “hydrated lime” will be understood to mean calcium hydroxide. In some examples, the hydrated lime may be provided as quicklime (calcium oxide) which hydrates when mixed with water to form the hydrated lime. The hydrated lime may be included in examples of the cement compositions, for example, to form a hydraulic composition with the silica source. For example, the hydrated lime may be included in a silica source-to-hydrated-lime weight ratio of about 10:1 to about 1:1 or a ratio of about 3:1 to about 5:1. Where present, the hydrated lime may be included in the cement compositions in an amount in the range of from about 10% to about 100% by weight of the silica source, for example. In some examples, the 7hydrated lime may be present in an amount ranging between any of and / or including any of about 10%, about 20%, about 40%, about 60%, about 80%, or about 100% by weight of the silica source. One of ordinary skill in the art, with the benefit of this disclosure, should recognize the appropriate amount of hydrated lime to include for a chosen application.
[0029] In some examples, the cement compositions may comprise a calcium source other than hydrated lime. In general, calcium and a high pH, for example a pH of 7.0 or greater, may be needed for certain cementitious reactions to occur. A potential advantage of hydrated lime may be that calcium ions and hydroxide ions are supplied in the same molecule. In another example, the calcium source may be Ca(NO ) or CaCl with the 3 2 2hydroxide being supplied form NaOH or KOH, for example. One of ordinary skill would understand the alternate calcium source and hydroxide source may be included in a cement composition in the same way as hydrated lime. For example, the calcium source and hydroxide source may be included in a silica source-to-hydrated-lime weight ratio of about 10:1 to about 1:1 or a ratio of about 3:1 to about 5:1. Where present, the alternate calcium source and hydroxide source may be included in the cement compositions in an amount in the range of from about 10% to about 100% by weight of the silica source, for example. In some examples, the alternate calcium source and hydroxide source may be present in an amount ranging between any of and / or including any of about 10%, about 20%, about 40%, about 60%, about 80%, or about 100% by weight of the silica source. One of ordinary skill in the art, with the benefit of this disclosure, should recognize the appropriate amount of alternate calcium source and hydroxide source to include for a chosen application.
[0030] A target silica lime ratio may be defined and a cement additive comprising two or more cement components may be identified that meets the silica lime ratio. In some examples, the target silica lime ratio may range from about 80 / 20 silica to free lime by weight to about 60 / 40 silica to free lime by weight, for example, be about 80 / 20 silica to free lime by weight, about 70 / 30 silica to free lime by weight, or about 60 / 40 silica to free lime by weight. The silica lime ratio may be determined by measuring the available silica and lime for a given cement component.
[0031] Other additives suitable for use in cementing operations also may be included in embodiments of the cement compositions. Examples of such additives include, but are not limited to: weighting agents, retarders, accelerators, activators, gas control a dditives, lightweight additives, gas-generating additives, mechanical-property-enhancing additives, lost-circulation materials, filtration-control additives, fluid-loss-control additives, defoaming agents, defoaming agents, foaming agents, transition time modifiers, dispersants, thixotropic 8additives, suspending agents, and combinations thereof. One of ordinary skill in the art, with the benefit of this disclosure, should be able to select an appropriate additive for a particular application.
[0032] As mentioned previously, in order to determine if two or more of t he aforementioned cement components are compatible, several lab tests may be run. Additionally, any potential synergistic effects of the cement component may not be knownunless several laboratory tests are performed. Typically, a known cement composition may be first formulated and tested for properties such as, for example, the 24 hour compressive strength, fluid loss, and thickening time. Then, varying amounts of additives may be added to a fresh batch of cement compositions and the tests are re-run. The results are gathered form each test and compared. A new set of tests may then run with n ew concentrations of additives, for example, to adjust properties of the cement composition. The process of testing various additives in varying concentrations may go on for several trials until an acceptable cement composition or compositions is formulated. An acceptable cement composition may be one that meets certain design requirements, such as compressive strength, fluid loss, and thickening time. The cement composition design process may be done in a heuristic manner leading to a cement composition that may have the required engineering properties but may not be optimized for cost. Additionally, silica sources such as, for example, cement kiln dust, have been previously used as either pure fillers or in some examples, reactive components, in Portland based cement compositions. CKD will contribute a portion of silica which requires a portion of lime to react. In methods of cement composition formulation described above, the heuristic process does not take into account the silica to lime ratio of a composition.
[0033] The method described herein may reduce or eliminate the heuristic search for by a process that identifies a cement additive through a process of m easuring and categorizing a variety of cement components referred to as reactivity mapping. Reactivitymapping may comprise several steps. One step may comprise measuring the physical and chemical properties of d ifferent materials through standardized tests. Another step may comprise categorizing the materials through analysis of data collected and the predicted effecton cement slurry properties. Yet another step may comprise utilizing the data to estimate material reactivity, improve cement performance, predict blend mechanical properties mathematically based on analytical results, and / or predict slurry d ensity d ependence of compressive strength.
[0034] Measuring physical and chemical properties of e ach selected cement component may comprise many laboratory techniques and procedures including, but not 9limited to, microscopy, spectroscopy, x-ray diffraction, x-ray f luorescence, particle size analysis, water requirement analysis, scanning electron microscopy, energy-dispersive X-ray spectroscopy, surface area, specific gravity analysis, thermogravimetric analysis, morphology analysis, infrared spectroscopy, ultraviolet-visible spectroscopy, mass spectroscopy, secondary ion mass spectrometry, electron energy m ass spectrometry, dispersive x-ray spectroscopy, auger electron spectroscopy, inductively coupled plasma analysis, thermal ionization mass spectroscopy, glow discharge mass spectroscopy x-ray p hotoelectron spectroscopy, mechanical property testing, Young’s Modulus testing, rheological properties, Poisson’s Ratio. One or more of the preceding tests may be consider API tests, as set forth in the API recommended practice for testing well cements (published as ANSI / API recommended practice 10B-2). Additional API tests not specifically listed above may also be used for the measurements. The physical and chemical properties may be measured for a group of cement components. Two or more of the cement components measured may be different types of cement components (e.g., volcanic rock, CKD, fly ash, etc.). Two or more of the cement components may be the same type but from different sources (e.g., volcanic rock from source 1, volcanic rock from source 2, etc.).
[0035] X-ray p owder diffraction is one analysis technique that may be used for measuring the physical and chemical properties of the cement components. X-ray powder diffraction is a technique of e xposing a sample to x-rays, neutrons, or electrons and measuring the amount of i nter-atomic-diffraction. The sample acts a diffraction grating thereby producing a differing signal at different angles. The typical properties that may be measured are the phase identification for the identification and characterization of a crystalline solid. Other properties may be crystallinity, lattice parameters, expansion tensors, bulk modulus, and phase transitions.
[0036] X-ray fluorescence is another analysis technique that may be used for measuring the physical and chemical properties of t he cement components. X-ray fluorescence may use short wave x-rays to ionize atoms in a sample thereby causing them to fluoresce at certain characteristic wavelengths. The characteristic radiation released by a sample may allow accurate identification of the component atoms in the sample as well as their relative amounts.
[0037] Particle size analysis is another analysis technique that may be used for measuring the physical and chemical properties of the cement components. Particle size analysis may be accomplished through analysis by various laboratory techniques including but not limited to laser diffraction, dynamic light scattering, static image analysis, and 10dynamic image analysis. Particle size analysis may also provide information about the morphology of a particular sample. Morphology may include parameters such as sphericity and roundness as well as the general shape of a particle such as disk, spheroid, blade, or roller. With a knowledge of the morphology and particle size, the average surface area and volume may be estimated. Surface area and volume may be important in determining the water requirement as well as reactivity. In general, a relatively smaller particle size may react more quickly than a relatively larger particle size. Also the relatively smaller particle size may have a greater water requirement to completely hydrate than a relatively larger particle size.
[0038] Energy dispersive x-ray spectroscopy is another analysis technique that may be used for measuring the physical and chemical properties of the cement components.Energy dispersive x-ray spectroscopy is an analytical technique used to analyze the elements present in a sample and determine the chemical characterization of a s ample. Other techniques may include Fourier transform infrared spectroscopy, ultraviolet-visible spectroscopy, mass spectroscopy, secondary ion mass spectrometry, electron energy mass spectrometry, dispersive x-ray s pectroscopy, auger electron spectroscopy, and x-ray photoelectron spectroscopy.
[0039] The cement components may be analyzed to determine their water requirement. Water requirement is typically defined as the amount of mixing water that is required to be added to a powdered, solid material to form a slurry of a specified consistency. Water requirement for a particular cement component may be determined by a process that includes a) preparing a Waring blender with a specified amount of water, b) agitating the water at a specified blender rpm, c) adding the powdered solid that is being investigated to the water until a specified consistency is obtained, and d) calculating the water requirement based on the ratio of water to solids required to reach the desired consistency.
[0040] The cement components may be analyzed to determine their specific surface area. Specific surface area generally refers to the total surface area and may be reported as the total surface area per unit mass. Values obtained for specific area are dependent on the analysis technique. Any suitable analysis technique may be used, including, but not limited to, adsorption based methods such as Brunauer-Emmett-Teller (BET) analysis, methylene blue staining, ethylene glycol monoethyl ether adsorption, and a protein-retention method, among other.
[0041] Thermogravimetric analysis is another analysis technique that may be used for measuring the physical and chemical properties of t he cement components.11Thermogravimetric analysis is a method of thermal analysis wherein changes in physical and chemical properties of a sample may be measured. In general the properties may be measured as a function of increasing temperature, such as with a constant heating rate, or as a function of time with a constant temperature or a constant mass change. Properties determined by thermogravimetric analysis may include first-order phase transitions and second-order phase transitions such as vaporization, sublimation, adsorption, desorption, absorption, chemisorption, desolvation, dehydration, decomposition, oxidation and reduction reactions, ferromagnetic transition, superconducting transition, and others.
[0042] In addition to determining physical and chemical properties of the cement components themselves, laboratory tests may also be run to determine behavior of the cement components in a cement composition. For example, the cement components may be analyzed in a cement composition to determine their compressive strength development and mechanical properties. For example, a preselected amount of the cement component may be combined with water and lime (if needed for setting). The mechanical properties of the cement composition may then be determined including, compressive strength, tensile strength, and Young’s modulus. Any of a variety of different conditions may be used for the testing so long as the conditions are consistent for the different cement components.
[0043] Compressive strength is generally the capacity of a material or structure to withstand axially directed pushing forces. T he compressive strength of t he cementcomponent may be measured at a specified time after the cement component has been mixed with water and the resultant cement composition is maintained under specified temperature and pressure conditions. For example, compressive strength can be measured at a time in the range of about 24 to about 48 hours (or longer) after the fluid is mixed and the fluid is maintained at a temperature of from 100 °F to about 200 °F and atmospheric pressure. Compressive strength can be measured by either a destructive method or non-destructive method. The destructive method physically tests the strength of treatment fluid samples at various points in time by crushing the samples in a compression-testing machine. The compressive strength is calculated from the failure load divided by the cross-sectional area resisting the load and is reported in units of pound-force per square inch (psi). Non-destructive methods typically may employ a n Ultrasonic Cement Analyzer (“UCA”), ®available from Fann Instrument Company, Houston, TX. Compressive strengths may be determined in accordance with A PI RP 10B-2, Recommended Practice for Testing Well Cements, First Edition, July 2005.12
[0044] Tensile strength is generally the capacity of a material to withstand loads tending to elongate, as opposed to compressive strength. The tensile strength of the cement component may be measured at a specified time after the cement component has been mixed with water and the resultant cement composition is maintained under specified temperature and pressure conditions. For example, tensile strength can be measured at a time in the range of about 24 to about 48 hours (or longer) after the fluid is mixed and the fluid is maintained at a temperature of from 100 °F to about 200 °F and atmospheric pressure. Tensile strength may be measured using any suitable method, including, but not limited to, in accordance with the procedure described in ASTM C307. That is, specimens may be prepared in briquette molds having the appearance of dog biscuits with a one square inch cross-sectional area at the middle. Tension may then be applied at the enlarged ends of t he specimens until the specimens break at the center area. The tension in pounds per square inch at which the specimen breaks is the tensile strength of the material tested.
[0045] Young’s modulus also referred to as the modulus of elasticity is a measure of the relationship of an applied stress to the resultant strain. In general, a highly deformable (plastic) material will exhibit a lower modulus when the confined stress is increased. Thus, the Young’s modulus is an elastic constant that demonstrates the ability of the tested material to withstand applied loads. A number of different laboratory techniques may be used to measure the Young’s modulus of a treatment fluid comprising a cementitious component after the treatment fluid has been allowed to set for a period of time at specified temperature and pressure conditions.
[0046] Although only some select laboratory techniques may have been mentioned, it should be understood that there may many analytical techniques that may be appropriate or not appropriate for a certain sample. One of ordinary skill in the art with the benefit of this disclosure should be able to select an appropriate analytical technique to determine a certain property of interest.
[0047] Once the analytical techniques have been performed on the cement components, the data may be categorized and correlated. Some categories may include, but are not limited to, specific surface area, morphology, specific gravity, water requirement, etc. In some examples, the components may be categorized by relative amounts, including amount of at least one following: silica, alumina, iron, iron, calcium, calcium, sodium, potassium, magnesium, sulfur, oxides thereof, and combinations thereof. For example, the components may be categorized based on an oxide analysis that includes without limitation, silica content, calcium oxide content, and alumina content among other oxides that may be 13present in the cement component.. In addition, correlations between the cement components may be generated based on the categorization of the data. For example, the various categories of properties may be plotted against one another. In some examples, water requirement versus specific surface area may be plotted. Accordingly, the water requirement of the cement component may be correlated to the specific surface area so that the specific surface area is a function of w ater requirement. Specific surface area may be used to predict reactivity of a cement component (or components). However, specific surface area may not always be available for each material as specific surface area analysis typically requires a specialized instrument. Accordingly, if the water requirement may be obtained for the cement component, the correlation between water requirement and specific surface area may be used to obtain an estimate for specific surface area, which may then be used to predict reactivity.In addition to correlations between specific surface area and reactivity, correlations may also be made between specific surface area and other mechanical properties such as tensile strength and Young’s modulus.
[0048] Some cement components that are alkali soluble may comprise reclaimed or natural materials. Specifically silica containing cement components may comprise materials such as mined materials, for example volcanic rock, perlite, waste materials, such as fly ashand CKD, and agricultural ashes as previously described. In some examples the cement component that is alkali soluble may have synergistic effects with a Portland cement while others may be incompatible. In some examples a cement component that is alkali soluble may cause gelation, high heat generation, water retention, among other effects. These and other effects may be realized during laboratory testing of the cement component in a cement composition comprising Portland cement. Laboratory equipment may be configured to detect the effects of the cement component on the composition. In some examples, equipment such a calorimeter may measure and quantify the amount of heat generation per unit mass of the cement component. Viscometers may measure the increase in gelation caused by the cement component. Each of the physical effects caused by the addition of the cement component may be measured at several concentrations and then categorized, e.g., plotted or mapped. Once a component is mapped, the effect of adding the component to a cement composition may be predicted by referencing the categorization.
[0049] As mentioned previously, some cement components that are alkali soluble may induce gelling when included in a cement composition. Although a higher gelling rate may be undesirable in some examples, in other examples, a higher gelling rate may be advantageous or necessary to meet the engineering design criteria. Usually one of ordinary 14skill in the art would select a suitable gelling agent or viscosifier for use in the cement composition. With the benefit of mapping, one of ordinary skill should be able to select a cement component that is alkali soluble that may serve a dual purpose. For example, a cement component may increase the compressive strength of a cement composition but also increase the gelling during mixing. If the engineering design criteria requires a higher gelling during mixing, it may be advantageous to include the cement component that increases thecompressive strength while also increasing gelling. The inclusion of a cement component that exhibits multiple effects may reduce the amount of additional additives, such as gelling agents or viscosifiers, needed, which may be high cost. Since the component’s gelling effect may have been documented in a map, the amount of component to include in a cement composition may be readily determined.
[0050] Another potentially advantageous physical effect that may be mapped is dispersing ability. Some cement components may comprise relatively spherical particles. The relatively spherical particles may exert a “roller bearing” effect in a cement composition with water. The effect may cause the other components in the cement composition to become more mobile thereby dispersing the components in the cement composition. Another potentially advantageous physical property that may be mapped is surface area. Surface area may relate to density wherein a relatively higher surface area particle may lower the density of a cement composition. Particles which lower the density may be used as a low density additive. Another potentially advantageous effect that may be mapped is particle size. Components with relatively smaller particle sizes may have the ability to form a filter cake against a formation thereby blocking cement from e scaping into a formation. Cement components with a small particle size may be used as a fluid loss control agent. With the benefit of the present disclosure, one of ordinary skill should be able to select a cement component and map its properties. One of ordinary skill should also be able to select a secondary property of interest of the cement component and with the benefit of the map, create a slurry with the desired properties.
[0051] Another potential benefit of replacing traditional cement additives with silica based cement components is a reduction in cost. A silica based cement component may partially or fully replace a relatively more expensive cement additive as discussed above. The cost of the cement composition may be improved by balancing the required engineering parameters such as compressive strength, mix ability, free water content, and others in order to maximize the amount of relatively lower cost silica based cement components. Any remaining deviation from the engineering requirement may be “made up” with the relatively 15more expensive cement additive. In this way, the cement composition may be reduced to a minimum cost per pound since the engineering requirements are met with a blend of primarily lower cost components.
[0052] Once the data is collected by the chosen laboratory techniques, categorized, and mapped, several operations may be performed on the data in order to yield predictions about a cement composition that comprises mapped cement components. Set properties, for example, may be estimated. A method of estimating the material reactivity based on the reactive index will be described below. Material reactivity may be based on many parameters such as specific surface area and specific gravity. Another use for the mapped data may be to improve cement slurry performance based on parameters such as particle shape, particle size, and particle reactivity. The data may also be used to predict and capture slurry density dependence of compressive strength and use the insight gathered to design improved cement formulations. The data may also be used to predict a c composition to achieve a just right cement formulation. The criteria for just right may be compressive strength, cost, rheology, mechanical properties, fluid loss control properties, thickening times, and others.
[0053] Reactivity mapping may be used to estimate various mechanical properties of a cement component, including compressive strength, tensile strength, and Young’s modulus. As previously described, correlations may be made between specific surface area and certain mechanical properties, such as reactivity, tensile strength, and Young’s modulus. Using these correlations the mechanical properties for a cement component or combination of cement components may be predicted.
[0054] One technique that may be used to correlate reactivity and specific surface area is the reactive index. Without being limited by theory, the reactive index of a cementcomponent may be referred to as a measure of the cement component’s reactivity as adjusted for differences in surface area. It is important to note that the term “cement component” refers to any material that is cementitious when mixed with w ater and / or lime and a suspending agent, when necessary, such that the slurry is stable. A “cementitious reactive index” can be defined as, but not limited to, Equation [1] as follows: ( ) = , , , [1] Where:16 = Unconfined UCS (ultimate compressive strength) obtained from samples cured at specific reference temperature, pressure and age. =Density of slurry that was prepared and cured for measuring UCS = Specific surface area obtained by typical particle size analysis methods.A “physicochemical index” (PCI) of the cementitious component may be defined as, but not limited to Equation [2]: = , , , , , , , , [2] Where: = Surface area of the cementitious component i, = specific gravity of the cementitious component i, = mass average or volume average diameter of the particle size distribution of cementitious component i, = Mass concentration of silica oxide of component i, = Mass concentration of calcium oxide of component i, = Mass concentration of Aluminum oxide of component i, = Mass concentration of sodium oxide of component i, = Mass concentration of iron oxide of component i,
[0055] It should be noted that the mass concentrations referenced above and here to for, may be measured, but is not limited to X-ray fluorescence spectroscopy measuring technique and a reference to “component i” is equivalent to “cementitious component i”. The functions in Equations [1] and [2] that define CRI and PCI , when properly defined, the i ifollowing universal relationship may hold for a wide range of cementitious materials such as, but not limited to, Portland cements; fly ash; other pozzolanic materials; other ashes; etc. ( ) [ ] = 3 FIG. 1 is a graph of Equation [1] versus Equation [2], illustrating the accuracy of Equations [1], [2] and [3] when applied to five different types of cementitious material sources and three 17samples of similar materials but from different sources. The simulated data was found to 0.2256 2have a relationship of y=36.252x , wherein R =0.9406.
[0056] In some examples, the form of Equation [3] may be a power law, such as in Equation 4. = { } [4] A and B are coefficients that may be unique the various species and sources of cementitious materials selected. Once the generalized function defined in Equation [4] is defined for a given population or group of cementitious components, a linear or nonlinear summation relationship further defined below, may be used in conjunction with Equation [5] to predict the UCS of various combinations of cementitious materials for specified slurry densities, temperatures, pressures and curing age. = { } [5] Where, is defined as the CRI for the unique combination of n cementitious components as the composite, and similarly is defined as the Physicochemical Index for the composite. A given composite with mass of is defined as: = + + + [6] Where: is defined as the mass fraction of the cementitious component i, and n is the total number of independent cementitious components. Once the function is defined in Equation [5], then the composite value of the physicochemical reactive index may be computed using Equation [7] as follows: = + + + ⋯ + [7]
[0057] Where: PCI is defined as the overall reactive index for a blend of n number of cuniquely independent cementitious components, is defined as the mass fraction of the 18cementitious component i, a nd n is the total n umber of i ndependent cementitious components. Once PCI has been determined for specific assumed blend of s elected ccementitious components, then the linear or non-linear summations (Equations [8] and [9]) are determined for the following terms: = + + + ⋯ + [8] and, = + + + … + [9] PCI is used to compute the value of using either Equation [5] or the more generalized c form o f Equation [3] for the composite terms. Once is determined for the given composite blend, then the composite values of and may be used along with Equation
[10] to predict the actual compressive strength of the composite blend, . ( ) = , , ,
[10]