Titanium diboride wettable cathode
Patent Information
- Application Number
- NO20241131
- Authority / Receiving Office
- NO · NO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-01-31
- Filing Date
- 2024-11-15
- Publication Date
- 2024-11-15
AI Technical Summary
Existing titanium diboride materials are difficult to apply to wettable cathodes. There are difficulties in preparing ceramic cathodes, high costs, and poor thermal shock resistance. Titanium diboride composite cathodes have high carbon content, high porosity, and short life. The titanium coating is easy to peel off and has a short lifespan.
It adopts a combined structure of titanium diboride cold-pressed sintered block and titanium diboride coating. Through carbon fiber reinforcement, titanium nitride assisted sintering, isostatic pressing and other measures, the cost is reduced and the strength and density are improved, and the surface is formed Titanium diboride coating, using plasma spraying technology.
It has achieved significant cost reduction, strong thermal shock resistance, unlimited structural size, and longer life. Its performance has reached a level similar to that of pure titanium diboride ceramics, meeting the needs of inert anodes and prebaked carbon anodes for aluminum electrolysis.
Abstract
Description
A titanium diboride wettable cathode
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This disclosure claims priority to Chinese patent application number 202310047908.7, filed on January 31, 2023, entitled “A Titanium Diboride Wettable Cathode,” the entire contents of which are incorporated herein by reference. Technical Field
[0003] The present disclosure relates to the field of aluminum electrolysis, and in particular to a titanium diboride wettable cathode. Background Art
[0004] Wettable cathodes are crucial for the development of both inert anode and prebaked carbon anode aluminum electrolysis. When using inert anodes, the aluminum electrolysis reaction equation transforms from Al2O3+C=Al+CO2 to Al2O3=Al+O2, and the theoretical decomposition voltage increases from 1.2V to 2.2V. This means the theoretical decomposition voltage of aluminum electrolysis using inert anodes is 1V higher than that using carbon anodes. To maintain the same or lower energy consumption as carbon anode aluminum electrolysis, inert anode aluminum electrolysis must be combined with wettable cathodes and employ an aluminum electrolysis cell with a vertical electrode structure. Currently, prebaked anode aluminum electrolysis has achieved significant energy reductions by reducing the voltage drop of peripheral conductors (e.g., anode, steel claws, cathode, cathode steel rod, peripheral busbar, etc.) and horizontal current. Using wettable cathodes to achieve "dry cathode" operation, i.e., eliminating the aluminum liquid layer, is an important option for the next stage of deep energy conservation. Without the fluctuation of the aluminum liquid layer and the heat loss of the aluminum liquid layer, the pole pitch can be less than 3.5cm or even lower, thereby greatly reducing the cell voltage and energy consumption.
[0005] Whether using inert anodes or carbon anodes for aluminum electrolysis, high requirements are placed on wettable cathodes in the absence of, or a thin, molten aluminum layer. First, good wettability is required, ensuring that molten aluminum can precipitate directly onto the wettable cathode surface. Second, without the protection of a molten aluminum layer, the cathode itself must be significantly more resistant to corrosion from electrolyte melts and sodium-potassium penetration.
[0006] Currently, titanium diboride (TiB2) is an ideal wettable cathode material. Pure titanium diboride offers excellent conductivity, high strength, wear resistance, and good wettability with molten aluminum. It also exhibits strong resistance to corrosion from electrolyte melts, molten aluminum, and sodium and potassium penetration. Existing wettable cathodes made from titanium diboride can be categorized into three main types: titanium diboride ceramic cathodes, titanium diboride composite cathode materials, and titanium diboride coatings. All three types of wettable cathodes present certain challenges: ceramic cathodes are difficult to prepare, costly, and exhibit poor thermal shock resistance, severely restricting their industrial application; titanium diboride composite cathode materials have high carbon content, high porosity, and a short lifespan; and titanium diboride coatings are prone to flaking and have a short lifespan. This makes titanium diboride difficult to use as a wettable cathode.
[0007] Summary of the Invention
[0008] The purpose of the present disclosure is to provide a titanium diboride wettable cathode, so as to solve the technical problem in the prior art that titanium diboride is difficult to be applied to wettable cathodes.
[0009] According to a first aspect of the present disclosure, a titanium diboride wettable cathode is provided, comprising: a titanium diboride cold-pressed sintered block, the titanium diboride cold-pressed sintered block comprising titanium diboride and additives, the additives comprising graphite, carbon fiber, and titanium nitride; and a titanium diboride coating applied to the surface of the titanium diboride cold-pressed sintered block.
[0010] According to the second aspect of the present disclosure, a method for preparing a titanium diboride wettable cathode is provided, and the method for preparing a titanium diboride wettable cathode comprises the following steps: mixing titanium diboride powder with additives, water, a dispersant, and a binder to form a slurry, wherein the additives include graphite, carbon fiber, and titanium nitride; spray-drying and granulating the slurry to obtain a powder; isostatically pressing the powder to obtain a compact; after processing and adjusting the shape and size of the compact, performing a high-temperature degreasing treatment on the compact at a first temperature and an inert atmosphere to obtain a degreased compact; densifying and sintering the degreased compact at a second temperature and an inert atmosphere to obtain a titanium diboride cold-pressed sintered block; using titanium diboride micropowder as a raw material, plasma spraying the surface of the titanium diboride cold-pressed sintered block to form a titanium diboride coating to obtain the titanium diboride wettable cathode. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] In order to more clearly illustrate the technical solutions in the embodiments of the present disclosure, a brief introduction will be given below to the drawings required for use in the description of the embodiments. Obviously, the drawings described below are some embodiments of the present disclosure. For ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.
[0012] FIG1 is a schematic flow diagram of a method for preparing a titanium diboride wettable cathode according to some embodiments of the present disclosure. DETAILED DESCRIPTION
[0013] The present disclosure will be described in detail below in conjunction with specific embodiments and examples, and the advantages and various effects of the present disclosure will be more clearly presented. It should be understood by those skilled in the art that these specific embodiments and examples are used to illustrate the present disclosure, rather than to limit the present disclosure.
[0014] Throughout the specification, unless otherwise specified, the terms used herein should be understood as meanings commonly used in the art. Therefore, unless otherwise defined, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art to which this disclosure pertains. In the event of a conflict, this specification takes precedence. Unless otherwise specified, the various raw materials, reagents, instruments and equipment used in this disclosure can be purchased commercially or can be obtained by existing methods.
[0015] Various embodiments of the present disclosure may be presented in the form of a range; it should be understood that the description in the form of a range is merely for convenience and brevity and should not be construed as a hard limitation on the scope of the present disclosure; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numbers within the range. For example, the description of a range from 1 to 6 should be considered to have specifically disclosed sub-ranges such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5, and 6, regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0016] In the present disclosure, unless otherwise stated, the directional words used, such as "upper" and "lower", refer specifically to the directions of the drawings in the accompanying drawings. In addition, in the description of the present disclosure, the terms "include", "comprise", etc. mean "including but not limited to". Moreover, the terms "include", "comprises" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device comprising a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In this article, relational terms such as "first" and "second" are merely used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of associated objects, indicating that there can be three relationships, for example, A and / or B can mean: the existence of A alone, the existence of A and B at the same time, and the existence of B alone. For the association relationship of more than three associated objects described by "and / or", it means that any one of the three associated objects can exist alone, or any at least two of them can exist at the same time. For example, for A, and / or B, and / or C, it can be expressed that any one of A, B, and C exists alone, or any two of them exist at the same time, or three of them exist at the same time. In this article, "at least one" refers to one or more, and "multiple" refers to two or more. "At least one", "the following at least one" or similar expressions refer to any combination of these items, including any combination of single or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all represent: a, b, c, a~b (i.e., a and b), a~c, b~c or a~b~c, where a, b, c can be single or multiple, respectively.
[0017] In a first aspect, an embodiment of the present disclosure provides a titanium diboride wettable cathode, which may include: a titanium diboride cold-pressed sintered block, which includes titanium diboride and additives, wherein the additives include graphite, carbon fiber, and titanium nitride; and a titanium diboride coating applied to the surface of the titanium diboride cold-pressed sintered block.
[0018] Carbon fiber can play a role in increasing the strength of the titanium diboride cold-pressed sintered block. Titanium nitride can assist in sintering. Those skilled in the art will understand that carbon-containing composite ceramic materials with titanium diboride as the main body are generally processed by hot pressing and sintering process. The hot pressing and sintering process is the key factor that leads to the high cost of titanium diboride-C composite hot-pressed ceramics, accounting for about 75% of the total cost. Therefore, the use of cold pressing and sintering instead of hot pressing and sintering in the present disclosure can greatly reduce the process cost. Compared with hot pressing and sintering, the density and strength of cold pressing and sintering will be relatively weaker. The present disclosure adopts carbon fiber reinforcement, titanium nitride assisted sintering, isostatic pressing and other measures to greatly improve the strength and density of cold-pressed sintered composite blocks, and also reduce the required sintering temperature. The cost of the present disclosure is much lower than the hot pressing process itself. The titanium diboride coating can be formed by plasma spraying, and its cost increase is related to the surface area. It is estimated to be less than 1,500 yuan / m 2 . Measures to improve the strength and density of the cold-pressed and sintered titanium diboride blocks themselves will only result in a relatively small increase in cost. Comprehensive calculations show that the cost of the present disclosure can be reduced by 30%, or even more than 50%, compared to carbon-containing titanium diboride hot-pressed ceramics. The present disclosure uses a low-carbon content cold-pressed and sintered titanium diboride block as a matrix, and further provides a titanium diboride coating on its surface, which can further reduce the porosity of the cathode surface and improve the overall performance of the cathode. Pure titanium diboride has the advantages of good electrical conductivity, high strength, wear resistance, and good wetting with aluminum water. It also has a strong ability to resist electrolyte melts, aluminum liquid corrosion, and sodium and potassium penetration. The present disclosure fully combines the advantages of the two, and the performance of the obtained titanium diboride in wetting the cathode surface reaches a level similar to that of pure titanium diboride ceramics.
[0019] In summary, the present invention discloses a low-carbon content titanium diboride wettable cathode having the following advantages: (1) compared with carbon-containing titanium diboride hot-pressed ceramic cathodes or pure titanium diboride ceramic cathodes, the preparation cost is greatly reduced; (2) compared with carbon-containing titanium diboride hot-pressed ceramic cathodes or pure titanium diboride ceramic cathodes, the structural size of the sample will not be restricted, the thermal shock resistance is strong, and it is easier to process; (3) compared with traditional titanium diboride-C composite cathodes and ordinary titanium diboride coating cathodes, the carbon content can be made very low and the density is high, the wettability with aluminum water and the resistance to electrolyte melt and sodium and potassium penetration are better, it is not easy to form an intercalation structure, and the service life is longer; (4) it can simultaneously meet the needs of inert anode aluminum electrolysis technology and prebaked carbon anode aluminum electrolysis technology for wettable cathodes under conditions of thin aluminum liquid layer or no aluminum liquid layer. The present invention significantly improves the strength and density of the cold-pressed sintered composite block by adopting measures such as carbon fiber reinforcement, titanium nitride assisted sintering, and isostatic pressing, while reducing the required sintering temperature. This allows the present invention to adopt a low-cost cold-pressed sintering process, and the structural size will not be restricted. It has strong thermal shock resistance and is easier to process. At the same time, a titanium diboride coating is provided on the surface of the titanium diboride cold-pressed sintered block, and the performance of the obtained titanium diboride in wettability of the cathode surface reaches a level similar to that of pure titanium diboride ceramics.
[0020] In some embodiments of the present disclosure, the titanium diboride cold-pressed sintered block comprises 16 to 19 parts of titanium diboride and 1 to 4 parts of additives, calculated by weight.
[0021] In some embodiments of the present disclosure, the additives include, based on the mass fraction of the additives, 0.1% to 2% of carbon fiber; 0.5% to 10% of titanium nitride; 0.5% to 5% of titanium oxide; and the balance being graphite.
[0022] The ratio of the above additives can make the titanium diboride wettable cathode have low carbon content and high density.
[0023] In some embodiments of the present disclosure, the thickness of the titanium diboride coating may be 200 to 1000 μm.
[0024] In a second aspect, an embodiment of the present disclosure provides a method for preparing a titanium diboride wettable cathode. The method for preparing a titanium diboride wettable cathode may include the following steps:
[0025] S1: mixing titanium diboride powder with additives, water, a dispersant, and a binder to form a slurry, wherein the additives include graphite, carbon fiber, and titanium nitride;
[0026] S2: spray drying and granulating the slurry to obtain a powder;
[0027] S3: isostatically pressing the powder to obtain a compact;
[0028] S4: After adjusting the shape and size of the compact, the compact is subjected to a high-temperature degreasing treatment at a first temperature and an inert atmosphere to obtain a degreased compact;
[0029] S5: densifying and sintering the degreased compact at a second temperature in an inert atmosphere to obtain a titanium diboride cold-pressed sintered compact;
[0030] S6: using titanium diboride fine powder as a raw material, plasma spraying the surface of the titanium diboride cold-pressed sintered block to form a titanium diboride coating, thereby obtaining the titanium diboride wettable cathode.
[0031] Those skilled in the art will appreciate that the method for preparing a titanium diboride wettable cathode can prepare the titanium diboride wettable cathode described in the first aspect. Therefore, the second aspect of the present disclosure has the beneficial effects of any embodiment of the first aspect, which will not be repeated here. The inert gas described in the present disclosure refers to at least one of nitrogen or a rare gas. Plasma spraying is conducive to the formation of a dense coating. Those skilled in the art will appreciate that before plasma spraying, the surface of the titanium diboride cold-pressed sintered block is generally roughened and cleaned, and the entire block is dried.
[0032] In some embodiments of the present disclosure, the mass ratio of the titanium diboride powder to the additive may be 16-19:1-4.
[0033] In some embodiments of the present disclosure, the additives may include, based on the mass fraction of the additives, 0.1% to 2% of carbon fiber; 0.5% to 10% of titanium nitride; 0.5% to 5% of titanium oxide; and the balance being graphite.
[0034] In some embodiments of the present disclosure, the first temperature may be 400-600°C; and / or, the second temperature may be 1250-1400°C; and / or, the time of the high-temperature degreasing treatment may be 4-6 hours; and / or, the pressure of the isostatic pressing treatment may be 120-200 MPa; and / or, the dispersant may be at least one of alcohol, polyacrylamide, and fatty acid polyethylene glycol ester; and / or, the binder may be polyvinyl alcohol.
[0035] In some embodiments of the present disclosure, the particle size d50 of the titanium diboride micropowder can be 15 to 25 μm; and / or, the plasma spraying can be atmospheric pressure plasma spraying or vacuum plasma spraying; and / or, the plasma spraying can be 10 to 50 μm thick each time, and the spraying can be completed in 5 to 20 times; and / or, the thickness of the titanium diboride coating can be 200 to 1000 μm; and / or, before the plasma spraying is carried out, the titanium diboride cold-pressed sintered block can be preheated to 100 to 200°C.
[0036] In some embodiments of the present disclosure, the plasma spraying is atmospheric pressure plasma spraying. During the plasma spraying, 5N high-purity argon can be used as the powder carrier gas, and 5N high-purity hydrogen or 5N high-purity helium can be used as the auxiliary gas.
[0037] Using 5N high-purity argon as the powder carrier gas and 5N high-purity hydrogen or 5N high-purity helium as the auxiliary gas can reduce the oxidation of titanium diboride powder during the high-temperature spraying process.
[0038] The present disclosure will be further described below with reference to specific examples. It should be understood that these examples are intended to illustrate the present disclosure only and are not intended to limit the scope of the present disclosure. Experimental methods in the following examples where specific conditions are not specified are generally measured in accordance with national standards. If no corresponding national standards are available, the methods were performed in accordance with commonly used international standards, conventional conditions, or conditions recommended by the manufacturer.
[0039] Example 1
[0040] 95wt% titanium diboride powder, 1wt% carbon fiber, 1wt% titanium nitride powder, 0.5wt% titanium oxide powder, and 2.5wt% graphite powder were mixed uniformly in a three-dimensional mixer. Pure water was added at a ratio of 1:1 to the weight of the materials, followed by polyacrylamide and polyvinyl alcohol solution, and ball milling was performed to form a slurry. Spray drying was used to granulate the mixture, and then the mixture was formed into a compact at 200MPa in an isostatic press. The compact was processed to obtain the desired cathode structure morphology. The processed compact was degreased at 600°C for 4 hours under a nitrogen atmosphere to obtain a degreased compact. The degreased compact was densified and sintered at 1400°C under an argon atmosphere to produce a titanium diboride cold-pressed sintered block. Testing and analysis showed that the titanium diboride cold-pressed sintered block had a porosity of 12.5% and a room-temperature flexural strength of 48MPa.
[0041] The resulting cold-pressed sintered titanium diboride block is surface-roughened, purified, and dried as a whole. Titanium diboride powder is used as raw material for atmospheric pressure plasma spraying. Its purity is greater than 98%, and its particle size d50 is 25 μm. Atmospheric pressure plasma spraying uses 5N high-purity argon as the carrier gas and 5N high-purity hydrogen as the auxiliary gas. Each spraying is 10 to 50 μm thick, and 20 sprayings are completed to form a titanium diboride coating. Before the first spraying, the substrate is preheated with a spray gun at approximately 160°C. Testing and analysis revealed that the titanium diboride coating has an oxygen content of 9.6%, a porosity of 8.4%, and a coating-substrate bonding strength of 6.7 N·mm. -2 .
[0042] The wettable cathode prepared according to the above process has a width * height * thickness = 10cm * 25cm * 3.5cm and is installed vertically at the bottom of the inert anode aluminum electrolytic cell. The actual working area is 200cm 2 *2, with two inert anodes, in KF-NaF-AlF3-Al2O3 electrolyte system, 820℃, 200A current, cathode current density 0.5A / cm 2 After running for 1000h under the same conditions, the cathode was intact and well wetted with aluminum water.
[0043] Example 2
[0044] 80wt% titanium diboride powder, 2wt% carbon fiber, 10wt% titanium nitride powder, 0.5wt% titanium oxide powder, and 7.5wt% graphite powder were mixed in a three-dimensional mixer; pure water was added at a ratio of 1:1 to the weight of the material, and fatty acid polyethylene glycol and polyvinyl alcohol solution were added, and ball milling was performed to form a slurry; spray drying was used for granulation, and then the granules were formed into compacts in an isostatic press at 180MPa, and the desired cathode structure morphology was obtained by processing the compacts; the processed compacts were degreased at 400°C for 6 hours under a nitrogen atmosphere to obtain degreased compacts; the degreased compacts were densified and sintered at 1350°C under an argon atmosphere to obtain titanium diboride cold-pressed sintered blocks. After testing and analysis, the porosity of the titanium diboride cold-pressed sintered blocks was 11.2% and the room-temperature flexural strength was 52MPa.
[0045] The resulting cold-pressed sintered titanium diboride block is surface-roughened, cleaned, and dried as a whole. Titanium diboride powder is used as raw material for atmospheric pressure plasma spraying. Its purity is greater than 98%, and its particle size d50 is 25 μm. Atmospheric pressure plasma spraying uses 5N high-purity argon as the carrier gas and 5N high-purity hydrogen as the auxiliary gas. Each spraying is 10 to 50 μm thick, and 20 sprayings are completed to form a titanium diboride coating. Before the first spraying, the substrate is preheated with a spray gun at approximately 120°C. Testing and analysis revealed that the titanium diboride coating has an oxygen content of 10.3%, a porosity of 8.8%, and a coating-substrate bonding strength of 6.4 N·mm. -2 .
[0046] The wettable cathode prepared according to the above process has a width * height * thickness = 10cm * 25cm * 3.5cm and is installed vertically at the bottom of the inert anode aluminum electrolytic cell. The actual working area is 200cm 2 *2, with two inert anodes, in KF-NaF-AlF3-Al2O3 electrolyte system, 820℃, 200A current, cathode current density 0.5A / cm 2 After running for 1000h under the same conditions, the cathode was intact and well wetted with aluminum water.
[0047] Example 3
[0048] 80wt% titanium diboride powder, 0.1wt% carbon fiber, 0.5wt% titanium nitride powder, 5wt% titanium oxide powder, and 14.4wt% graphite powder were mixed uniformly in a three-dimensional mixer; pure water was added at a ratio of 1:1 to the weight of the material, and fatty acid polyethylene glycol ester and polyvinyl alcohol solution were added, and ball milling was performed to form a slurry; spray drying was used for granulation, and then formed into a compact in an isostatic press at 160MPa, and the compact was processed to obtain the desired cathode structure morphology; the processed compact was degreased at 500℃ for 4h under a nitrogen atmosphere to obtain a degreased compact; the degreased compact was densified and sintered at 1350℃ under an argon atmosphere to produce a titanium diboride cold-pressed sintered block. After testing and analysis, the titanium diboride cold-pressed sintered block had a porosity of 11.8% and a room-temperature flexural strength of 44MPa.
[0049] The obtained titanium diboride cold-pressed sintered block is surface-roughened, purified, and dried as a whole; titanium diboride powder is provided as raw material for atmospheric pressure plasma spraying, with a purity greater than 98% and a particle size d50 of 25 μm. Atmospheric pressure plasma spraying uses 5N high-purity argon as the powder carrier gas and 5N high-purity hydrogen as the auxiliary gas; the thickness of each spray is 10 to 50 μm, and the titanium diboride coating is formed by spraying 20 times; before the first spraying, the substrate material is preheated with a spray gun at a preheating temperature of approximately 200°C. After testing and analysis, the titanium diboride coating has an oxygen content of 11.2%, a porosity of 9.2%, and a bonding strength of 5.8 N·mm -2 .
[0050] A wettable cathode block with an inclined surface prepared according to the above process has a rectangular orthographic projection surface of length * width = 20 cm * 15 cm. It is installed at the bottom of a laboratory-scale carbon anode aluminum electrolytic cell with a height of 12 cm at one end and 10 cm at the other end, forming an inclined shape. It is combined with a carbon anode with the same inclined angle to form a guide trough structure. The actual electrode working area is 300 cm 2 In the KF-NaF-AlF3-Al2O3 electrolyte system, 820℃, 240A current, cathode current density 0.8A / cm 2 The cathode was intact and well wetted with aluminum water under the conditions of 48h.
[0051] Example 4
[0052] 80wt% titanium diboride powder, 1wt% carbon fiber, 5wt% titanium nitride powder, 2wt% titanium oxide powder, and 12wt% graphite powder were mixed uniformly in a three-dimensional mixer; pure water was added at a ratio of 1:1 to the weight of the materials, and fatty acid polyethylene glycol ester and polyvinyl alcohol solution were added, and ball milling was performed to form a slurry; spray drying was used for granulation, and then formed into a compact in an isostatic press at 180MPa, and the compact was processed to obtain the desired cathode structure morphology; the processed compact was degreased at 600℃ for 4 hours under a nitrogen atmosphere to obtain a degreased compact; the degreased compact was densified and sintered at 1400℃ under an argon atmosphere to produce a titanium diboride cold-pressed sintered block. After testing and analysis, the titanium diboride cold-pressed sintered block had a porosity of 10.2% and a room-temperature flexural strength of 63MPa.
[0053] The resulting cold-pressed sintered titanium diboride block is surface-roughened, cleaned, and dried as a whole. Titanium diboride powder is used as raw material for atmospheric pressure plasma spraying. Its purity is greater than 98%, and its particle size d50 is 25 μm. Atmospheric pressure plasma spraying uses 5N high-purity argon as the carrier gas and 5N high-purity hydrogen as the auxiliary gas. Each spraying is 10 to 50 μm thick, and 20 sprayings are completed to form a titanium diboride coating. Before the first spraying, the substrate is preheated with a spray gun at approximately 180°C. Testing and analysis show that the titanium diboride coating has an oxygen content of 9.2%, a porosity of 8.4%, and a coating-substrate bonding strength of 7.5 N·mm. -2 .
[0054] The wettable cathode prepared according to the above process has a width * height * thickness = 10cm * 25cm * 3.5cm and is installed vertically at the bottom of the inert anode aluminum electrolytic cell. The actual working area is 200cm 2 *2, with two inert anodes, in KF-NaF-AlF3-Al2O3 electrolyte system, 820℃, 200A current, cathode current density 0.5A / cm 2 After running for 1000h under the same conditions, the cathode was intact and well wetted with aluminum water.
[0055] Example 5
[0056] 85wt% titanium diboride powder, 1wt% carbon fiber, 5wt% titanium nitride powder, 0.5wt% titanium oxide powder, and 8.5wt% graphite powder were mixed uniformly in a three-dimensional mixer; pure water was added at a ratio of 1:1 to the weight of the materials, and fatty acid polyethylene glycol ester and polyvinyl alcohol solution were added, and ball milling was performed to form a slurry; spray drying was used for granulation, and then formed into a compact in an isostatic press at 180MPa, and the compact was processed to obtain the desired cathode structure morphology; the processed compact was degreased at 600℃ for 4h under a nitrogen atmosphere to obtain a degreased compact; the degreased compact was densified and sintered at 1350℃ under an argon atmosphere to produce a titanium diboride cold-pressed sintered block. After testing and analysis, the titanium diboride cold-pressed sintered block had a porosity of 10.8% and a room-temperature flexural strength of 58MPa.
[0057] The resulting cold-pressed sintered titanium diboride block is surface-roughened, cleaned, and dried. Titanium diboride powder, with a purity greater than 98% and a particle size d50 of 25 μm, is used as raw material for atmospheric pressure plasma spraying. 5N high-purity argon is used as the carrier gas for atmospheric pressure plasma spraying, and 5N high-purity hydrogen is used as the auxiliary gas. Each spraying is applied with a thickness of 10 to 50 μm, and the titanium diboride coating is formed after 20 sprayings. Before the first spraying, the substrate is preheated with a spray gun at approximately 200°C. Testing and analysis revealed that the titanium diboride coating has an oxygen content of 10.5%, a porosity of 8.6%, and a coating-substrate bonding strength of 7.8 N·mm. -2 .
[0058] A wettable cathode block with an inclined surface prepared according to the above process has a rectangular orthographic projection surface of length * width = 20 cm * 15 cm. It is installed at the bottom of a laboratory-scale carbon anode aluminum electrolytic cell with a height of 12 cm at one end and 10 cm at the other end, forming an inclined shape. It is combined with a carbon anode with the same inclined angle to form a guide trough structure. The actual electrode working area is 300 cm 2 In the KF-NaF-AlF3-Al2O3 electrolyte system, 820℃, 240A current, cathode current density 0.8A / cm 2 The cathode was intact and well wetted with aluminum water under the conditions of 48h.
[0059] Some embodiments of the present disclosure have the following advantages over the prior art: the titanium diboride wettable cathode provided in the embodiments of the present disclosure greatly improves the strength and density of the cold-pressed sintered composite block by adopting measures such as carbon fiber reinforcement, titanium nitride assisted sintering, and isostatic pressing, while reducing the required sintering temperature, so that the present disclosure can adopt a low-cost cold-pressed sintering process, and the structural size will not be restricted, the thermal shock resistance is strong, and it is easier to process; at the same time, a titanium diboride coating is provided on the surface of the titanium diboride cold-pressed sintered block, and the performance of the titanium diboride wettable cathode surface obtained reaches a level similar to that of pure titanium diboride ceramics.
[0060] The foregoing description is intended only to provide specific embodiments of the present disclosure, intended to enable those skilled in the art to understand and implement the present disclosure. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present disclosure. Therefore, the present disclosure is not to be limited to the embodiments shown herein, but is to be construed in the broadest manner consistent with the principles and novel features claimed herein.
Claims
1. A titanium diboride wettable cathode comprising: A titanium diboride cold-pressed sintered block, wherein the titanium diboride cold-pressed sintered block comprises titanium diboride and additives, wherein the additives comprise graphite, carbon fiber, and titanium nitride; The titanium diboride coating is coated on the surface of the titanium diboride cold-pressed sintered block.
2. The titanium diboride wettable cathode according to claim 1, wherein In parts by weight, the titanium diboride cold-pressed sintered block comprises 16 to 19 parts of titanium diboride and 1 to 4 parts of additives.
3. The titanium diboride wettable cathode according to claim 2, wherein Calculated by mass fraction of the additives, the additives include: 0.1% to 2% of carbon fiber; 0.5% to 10% of titanium nitride; 0.5% to 5% of titanium oxide; and the balance being graphite.
4. The titanium diboride wettable cathode according to claim 1, wherein The thickness of the titanium diboride coating is 200-1000 μm.
5. A method for preparing a titanium diboride wettable cathode, comprising: Mixing titanium diboride powder with additives, water, a dispersant, and a binder to form a slurry, wherein the additives include graphite, carbon fiber, and titanium nitride; spray drying and granulating the slurry to obtain a powder; isostatically pressing the powder to obtain a compact; After the shape and size of the compact are adjusted by processing, the compact is subjected to a high-temperature degreasing treatment at a first temperature and in an inert atmosphere to obtain a degreased compact; Densification sintering the degreased compact at a second temperature and in an inert atmosphere to obtain a titanium diboride cold-pressed sintered compact; Titanium diboride fine powder is used as a raw material, and plasma spraying is performed on the surface of the titanium diboride cold-pressed sintered block to form a titanium diboride coating, thereby obtaining the titanium diboride wettable cathode.
6. The method for preparing a titanium diboride wettable cathode according to claim 5, wherein: The mass ratio of the titanium diboride powder to the additive is 16-19:1-4.
7. The method for preparing a titanium diboride wettable cathode according to claim 6, wherein: Calculated by mass fraction of the additives, the additives include: 0.1% to 2% of carbon fiber; 0.5% to 10% of titanium nitride; 0.5% to 5% of titanium oxide; and the balance being graphite.
8. The method for preparing a titanium diboride wettable cathode according to claim 5, wherein: The first temperature is 400-600° C.; and / or, The second temperature is 1250° C. to 1400° C.; and / or, The high temperature degreasing treatment time is 4 to 6 hours; and / or, The isostatic pressing treatment has a pressure of 120-200 MPa; and / or, The dispersant is at least one of alcohol, polyacrylamide, and fatty acid polyethylene glycol ester; and / or, The binder is polyvinyl alcohol.
9. The method for preparing a titanium diboride wettable cathode according to claim 5, wherein: The particle size d50 of the titanium diboride powder is 15 to 25 μm; and / or, The plasma spraying is atmospheric pressure plasma spraying or vacuum plasma spraying; and / or, The plasma spraying is performed with a thickness of 10 to 50 μm each time and the spraying is completed in 5 to 20 times; and / or, The thickness of the titanium diboride coating is 200 to 1000 μm; and / or, Before the plasma spraying is performed, the titanium diboride cold-pressed sintered block is preheated to 100-200°C.
10. The method for preparing a titanium diboride wettable cathode according to any one of claims 5 to 9, wherein: The plasma spraying is atmospheric pressure plasma spraying. When the plasma spraying is performed, 5N high-purity argon is used as the powder carrier gas, and 5N high-purity hydrogen or 5N high-purity helium is used as the auxiliary gas.