Resin compositions, cured materials, prepregs, foil-coated laminates, resin composites, printed wiring boards, and semiconductor devices.
Patent Information
- Application Number
- TW112109104
- Authority / Receiving Office
- TW · TW
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-03-14
- Filing Date
- 2023-03-13
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2043-03-12
AI Technical Summary
The resin with an indene skeleton described in prior art is not sufficiently hardened and requires a resin composition with excellent formability and low dielectric loss tangent (Df) for improved printed wiring boards and semiconductor devices.
A resin composition is developed by blending polyphenylene ether compounds with a carbon-carbon unsaturated double bond and a specific ratio of aromatic vinyl polymers, including a resin with an indene skeleton, to enhance formability and reduce dielectric loss tangent.
The resin composition achieves improved formability and low dielectric loss tangent, resulting in better performance of cured products, prepregs, metal foil-clad laminates, resin composite sheets, and semiconductor devices.
Smart Images

Figure TWG2TB001920151_001 
Figure TWG2TB001920151_002
Abstract
Description
[Technical Field]
[0001] This invention relates to resin compositions, cured materials, prepregs, metal foil laminates, resin composite sheets, printed wiring boards, and semiconductor devices. [Previous Technology]
[0002] In recent years, the integration and miniaturization of semiconductor components used in electronic devices and communication equipment, primarily mobile terminals, have accelerated. This necessitates technologies capable of high-density mounting of semiconductor components, demanding improvements in printed circuit boards (PCBs), which play a crucial role. Furthermore, the applications of electronic devices are becoming increasingly diversified and expanding. Corresponding to this trend, the various characteristics required of PCBs, their metal-clad laminates, prepregs, and the like have become more diverse and stringent. To obtain improved PCBs that take these requirements into account, various materials and processing methods have been proposed. One example is the improved development of resin materials constituting the prepreg and resin composite sheets.
[0003] Patent Document 1 discloses a resin having isopropenylphenyl terminals and a dihydroindene backbone, which is ideal for semiconductor sealing materials and printed circuit boards. [Prior Art Documents] [Patent Documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 2021-143333 [Summary of the Invention]
[0005] (The problem the invention aims to solve)
[0006] However, the resin with a dihydroindene backbone described in Patent Document 1 described above will not cure sufficiently if used directly. Therefore, novel resin compositions blended with other compounds, especially thermosetting compounds, are sought. In particular, resin compositions with excellent formability and low dielectric loss tangent (Df) are sought. The present invention aims to solve this problem and provides resin compositions with excellent formability and low dielectric loss tangent (Df), as well as cured products, prepregs, metal-coated laminates, resin composites, printed wiring boards, and semiconductor devices. (Solution to the problem)
[0007] Based on the above-mentioned problems, the inventors of this case conducted research and found that by blending a polyphenylene ether compound with carbon-carbon unsaturated double bonds at the end and a predetermined aromatic vinyl polymer in a specific ratio into a resin having an isopropenyl group at the end and a dihydroindene skeleton, the above-mentioned problems can be solved. Specifically, the above-mentioned problems can be solved by the following means. <1> A resin composition, relative to 100 parts by mass of a resin (A) having a terminal group represented by formula (T1) and a dihydroindene skeleton, contains 10 to 300 parts by mass of a polyphenylene ether compound (B) having a terminal carbon-carbon unsaturated double bond, and 10 to 300 parts by mass of a polymer having a constituent unit represented by formula (V), [Chemical 1] In formula (T1), Mb independently represents a hydrocarbon group with 1 to 12 carbon atoms that can also be substituted by halogen atoms, y represents an integer from 0 to 4, and * represents the bonding position with other sites, [Chemical 2] In formula (V), Ar represents an aromatic hydrocarbon linking group. * indicates the bonding position. <2> The resin composition as in <1>, wherein the resin (A) contains the resin represented by formula (T1-1), [Chemical 3] In formula (T1-1), R is the base containing the constituent unit represented by formula (Tx), Mb each independently represents a hydrocarbon group with 1 to 12 carbon atoms that can be substituted by halogen atoms, y is an integer from 0 to 4, [Chemical 4] In formula (Tx), n, o, and p are the average number of repeating units, n represents a number greater than 0 and less than 20, o and p each independently represent a number from 0 to 20, 1.0≦n+o+p≦20.0, Ma each independently represents a hydrocarbon group with 1 to 12 carbon atoms that can be substituted by halogen atoms, x represents an integer from 0 to 4, the constituent units (a), (b), and (c) are bonded by * and the constituent units (a), (b), (c), or other groups, and each constituent unit can also be bonded randomly. <3> The resin composition as in <1> or <2>, wherein the polyphenylene ether compound (B) with carbon-carbon unsaturated double bonds at the end contains a polyphenylene ether compound represented by formula (OP), [Chemical 5] In formula (OP), X represents an aromatic group, -(YO)n1- represents a polyphenylene ether structure, n1 represents an integer from 1 to 100, n2 represents an integer from 1 to 4, Rx is a group represented by formula (Rx-1) or formula (Rx-2), [Chemical 6] In formulas (Rx-1) and (Rx-2), R1, R2, and R3 each independently represent a hydrogen atom, alkyl, alkenyl, or alkynyl group, * represents a bonding site with an oxygen atom, Mc each independently represents a hydrocarbon group with 1 to 12 carbon atoms, z represents an integer from 0 to 4, and r represents an integer from 1 to 6.<4> A resin composition as described in any of <1> to <3>, wherein the polyphenylene ether compound (B) having a carbon-carbon unsaturated double bond at the end contains a polyphenylene ether compound represented by formula (OP-1), [Chemical 7] In formula (OP-1), X represents an aromatic group, -(YO)n 2- represents a polyphenylene ether structure, R1, R2, and R3 each independently represent a hydrogen atom, alkyl, alkenyl, or alkynyl group, n1 represents an integer from 1 to 6, n2 represents an integer from 1 to 100, and n3 represents an integer from 1 to 4. <5> A resin composition as described in any of <1> to <4>, wherein the polyphenylene ether compound (B) having a carbon-carbon unsaturated double bond at the end has a number average molecular weight (Mn) of 500 to 3000 and a weight average molecular weight (Mw) of 800 to 6000. <6> A resin composition as described in any one of <1> to <5>, wherein the number average molecular weight (Mn) of the resin (A) is 400 to 3000. <7> A resin composition as described in any one of <1> to <6>, wherein the mass ratio of resin (A) is 10 to 50 parts by mass relative to a total of 100 parts by mass of the resin (A) and the polyphenylene ether compound (B) having carbon-carbon unsaturated double bonds at the ends. <8> A resin composition as described in any one of <1> to <7> substantially does not contain polymerization inhibitors. <9> A resin composition as described in any one of <1> to <8> further contains the resin (A), the polyphenylene ether compound (B) having carbon-carbon unsaturated double bonds at the ends, and other compounds (C) besides the polymer having the constituent unit represented by formula (V). <10> The resin composition of <9>, wherein the other compound (C) contains one or more compounds selected from the group consisting of maleimide compounds, cyanate compounds, epoxy compounds, phenol compounds, compounds containing (meth)allyl groups, oxetane resins, benzo[a] compounds, arylcyclobutene resins, polyamide resins, polyimide resins, perfluoroethylene ether resins, styrene compounds other than the polyphenylene ether compound (B) with a carbon-carbon unsaturated double bond at the end, isopropylene compounds other than the resin (A) with a dihydroindene skeleton, polyfunctional (meth)acrylate compounds other than the polyphenylene ether compound (B) with a carbon-carbon unsaturated double bond at the end, elastomers, and petroleum resins. <11> A resin composition as described in any one of <1> to <10>, wherein the total content of the resin (A) and the polyphenylene ether compound (B) having carbon-carbon unsaturated double bonds at the ends is 40 parts by mass or more, relative to 100 parts by mass of the resin solids in the resin composition. <12> A resin composition as described in any one of <1> to <11> further comprises a filler (D). <13> A resin composition as described in <12>, wherein the content of the filler (D) is 10 to 1000 parts by mass, relative to 100 parts by mass of the resin solids in the resin composition.<14> A resin composition as described in any one of <1> to <13>, wherein the resin (A) contains a resin represented by formula (T1-1), the polyphenylene ether compound (B) having carbon-carbon unsaturated double bonds at the ends contains a polyphenylene ether compound represented by formula (OP-1), the polyphenylene ether compound (B) having a number average molecular weight (Mn) of 500-3000 and a weight average molecular weight (Mw) of 800-6000, the resin (A) having a number average molecular weight (Mn) of 400-3000, and the resin (A) having a mass ratio of 10-50 parts by mass relative to a total of 100 parts by mass of the resin (A) and the polyphenylene ether compound (B) having carbon-carbon unsaturated double bonds at the ends, and substantially does not contain polymerization inhibitors. Relative to 100 parts by mass of the resin solids in the resin composition, the total content of the resin (A) and the polyphenylene ether compound (B) with carbon-carbon unsaturated double bonds at the end is 40 parts by mass or more. [Chemical 8] In formula (T1-1), R is a base containing the constituent unit represented by formula (Tx), Mb independently represents a hydrocarbon group with 1 to 12 carbon atoms that can also be substituted by halogen atoms, and y is an integer from 0 to 4. In formula (Tx) of [Chemical Engineering 9], n, o, and p are the average number of repeating units, n represents a number greater than 0 and less than 20, o and p each independently represent a number from 0 to 20, 1.0≦n+o+p≦20.0, Ma each independently represents a hydrocarbon group with 1 to 12 carbon atoms that can also be substituted by halogen atoms, x represents an integer from 0 to 4, the constituent units (a), (b), and (c) are respectively bonded by * and the constituent units (a), (b), (c), or other groups, and each constituent unit can also be randomly bonded. In formula (OP-1) of [Chemical Engineering 10], X represents an aromatic group, -(YO)n 2- represents a polyphenylene ether structure, R 1, R 2, and R 3 each independently represent a hydrogen atom, alkyl, alkenyl, or alkynyl group, n 1 represents an integer from 1 to 6, n 2 represents an integer from 1 to 100, and n 3 represents an integer from 1 to 4. <15> A cured form of a resin composition as described in any one of <1> to <14>. <16> A prepreg formed from a substrate and a resin composition as described in any one of <1> to <14>. <17> A metal foil laminate comprising at least one layer formed of a prepreg as described in <16>, and metal foil disposed on one or both sides of the layer formed of the prepreg. <18> A resin composite sheet comprising a support and a layer formed of a resin composition as described in any one of <1> to <14> disposed on the surface of the support. <19> A printed wiring board comprising an insulating layer and a conductor layer disposed on the surface of the insulating layer, the insulating layer containing a layer formed of a resin composition as described in any one of <1> to <14>. <20> A semiconductor device comprising a printed wiring board as described in <19>. (Effects of the invention).
[0008] According to the present invention, resin compositions with excellent formability and low dielectric loss tangent (Df) can be provided, as well as cured materials, prepregs, metal foil laminates, resin composites, printed wiring boards, and semiconductor devices.
Implementation Method
[0010] The following describes this embodiment (hereinafter simply referred to as "this embodiment"). Furthermore, the following embodiment is used to illustrate the present invention, and the present invention is not limited to this embodiment. Also, in this specification, "~" is used to include the numerical values described before and after it as lower and upper limits. In this specification, various physical property values and characteristic values, unless specifically stated, are physical property values and characteristic values at 23°C. In the description of the base (atomic group) in this specification, the expressions for substitution and non-substitution are not specified, and include both unsubstituent and substituent bases (atomic groups). For example, "alkyl" includes not only unsubstituent alkyl groups (unsubstituted alkyl groups) but also substituent alkyl groups (substituted alkyl groups). In this specification, the absence of expressions for substitution and non-substitution means that non-substitution is preferred. In this specification, "(meth)allyl" refers to either or both allyl and methallyl; "(meth)acrylate" refers to either or both acrylate and methacrylate; "(meth)acrylate" represents either or both acrylate and methacrylate; and "(meth)acryl" represents either or both acrylonitrile and methacrylonitrile. In this specification, "step" is not necessarily an independent step; when it cannot be clearly distinguished from other steps, it is included in this terminology as long as it achieves the expected effect. Unless otherwise specified, the specifications and measurement methods described in this specification are based on the specifications as of January 1, 2022.
[0011] In this specification, the term "solid resin component" refers to the component excluding fillers and solvents, including resin (A) and polyphenylene ether compound (B), polymers having constituent units represented by formula (V), and other compounds (C) as needed, as well as other resin additive components (flame retardants and other additives). In this specification, relative permittivity and dielectric constant are used with the same meaning.
[0012] The resin composition of this embodiment comprises a resin (A) having a terminal group represented by formula (T1) and having a dihydroindene skeleton (also simply referred to as "resin (A)"), a polyphenylene ether compound (B) having a carbon-carbon unsaturated double bond at the end (also simply referred to as "polyphenylene ether compound (B)"), and a polymer having a constituent unit represented by formula (V). Specifically, the resin composition of this embodiment is characterized by containing, relative to 100 parts by mass of the resin (A) having a terminal group represented by formula (T1) and having a dihydroindene skeleton, 10 to 300 parts by mass of the polyphenylene ether compound (B) having a carbon-carbon unsaturated double bond at the end, and 10 to 300 parts by mass of the polymer having a constituent unit represented by formula (V). [Chemical 11] In formula (T1), Mb independently represents a hydrocarbon group with 1 to 12 carbon atoms that can also be substituted by halogen atoms, and y represents an integer from 0 to 4. * indicates the bonding position with other sites. [Chemical Engineering 12] In formula (V), Ar represents an aromatic hydrocarbon linker. * indicates the bonding position. [Chemical Engineering 13] In formula (T1), Mb independently represents hydrocarbon groups with 1 to 12 carbon atoms that can also be substituted with halogen atoms, and y represents an integer from 0 to 4. * indicates the bonding position with other sites. With this configuration, a resin composition with excellent formability and low dielectric loss tangent (Df) when made into a cured product can be obtained. Resin (A) having the terminal group represented by formula (T1) and having a dihydroindene backbone is not easy to polymerize when used alone. Furthermore, if it is not used in combination with a compound that is compatible with resin (A), phase separation is likely to occur. In this embodiment, by blending a polyphenylene ether compound (B) with a carbon-carbon unsaturated double bond at the end and a polymer having the constituent unit represented by formula (V) into resin (A) at a predetermined ratio, it is presumed that compatibility is improved, and a resin composition with excellent formability can be obtained. Furthermore, since resin (A) has a dihydroindene backbone, it is presumed that a resin composition with a low dielectric loss tangent (Df) when forming a cured product can be obtained. Also, by using a polymer having constituent units represented by formula (V), it is presumed that the dielectric loss tangent (Df) of the obtained cured product can be even lower. Moreover, in this embodiment, a resin composition with low melt viscosity can be obtained. Low melt viscosity, for example, even when combined with resins with high melt viscosity and poor formability, can reduce the minimum melt viscosity and improve formability. Furthermore, in this embodiment, a resin composition with high heat resistance can be obtained.
[0013] <Resin (A) having a terminal group represented by formula (T1) and a dihydroindene skeleton> The resin composition of this embodiment includes a resin (A) having a terminal group represented by formula (T1) and a dihydroindene skeleton. By using resin (A), a resin composition with excellent low dielectric properties (Dk and / or Df) can be obtained [Chemical 14] In formula (T1), Mb independently represents a hydrocarbon group with 1 to 12 carbon atoms that can also be substituted by halogen atoms, and y represents an integer from 0 to 4. * indicates the bonding position with other sites.
[0014] In formula (T1), Mb is preferably a hydrocarbon group with 1 to 10 carbon atoms that can be substituted with halogen atoms, more preferably a hydrocarbon group with 1 to 5 carbon atoms that can be substituted with halogen atoms, and even more preferably a hydrocarbon group with 1 to 3 carbon atoms that can be substituted with halogen atoms. Examples of halogen atoms include fluorine, chlorine, and bromine atoms, with fluorine or chlorine atoms being preferred. Mb is preferably a hydrocarbon group with 1 to 12 carbon atoms that has not been substituted with halogen atoms. The aforementioned hydrocarbon group is preferably an alkyl group, and a straight-chain alkyl group is even more preferred. Mb is preferably methyl or ethyl.
[0015] It is better for y to be an integer from 0 to 3, even better if it is an integer from 0 to 2, even better if it is 0 or 1, and even more ideal if it is 0.
[0016] In resin (A), each resin molecule may have terminal groups represented by formula (T1) at all its ends, or only a portion of its ends may have terminal groups represented by formula (T1). In resin molecules of resin (A), it is preferable to have 2 terminal groups represented by formula (T1).
[0017] Resin (A) has a dihydroindene backbone. It is not particularly limited that at least one molecule of resin in resin (A) has at least one dihydroindene backbone, but it is preferable that each molecule of resin (A) contains at least one dihydroindene backbone, and more preferably 1 to 20. This configuration tends to enhance the effects of the present invention.
[0018] It is preferable that the resin (A) contains the constituent units represented by the following formula (Txn). [Chemical 15] In formula (Txn), n is the average number of repeating units, which is a number greater than 0 and less than 20. Ma independently represents hydrocarbon groups with 1 to 12 carbon atoms that can also be substituted by halogen atoms. x represents an integer from 0 to 4.
[0019] In formula (Txn), each Ma is preferably a hydrocarbon group with 1 to 10 carbon atoms that can be substituted with halogen atoms, more preferably a hydrocarbon group with 1 to 5 carbon atoms that can be substituted with halogen atoms, and even more preferably a hydrocarbon group with 1 to 3 carbon atoms that can be substituted with halogen atoms. Examples of halogen atoms include fluorine, chlorine, and bromine atoms, with fluorine or chlorine atoms being preferred. Each Ma is preferably a hydrocarbon group with 1 to 12 carbon atoms that has not been substituted with halogen atoms. The aforementioned hydrocarbon group is preferably an alkyl group, and more preferably a straight-chain alkyl group. Ma is especially preferred to be methyl or ethyl.
[0020] It is better for x to be an integer between 0 and 3, even better if it is an integer between 0 and 2, better if it is 0 or 1, and even more ideal if it is 0.
[0021] Resin (A) is preferably a resin represented by formula (T1-1), and even more preferably a resin represented by formula (T1-1-2). [Chemical 16] In formula (T1-1), R is a base of a constituent unit represented by formula (Tx). Mb independently represents a hydrocarbon group with 1 to 12 carbon atoms that can be substituted by halogen atoms. y is an integer from 0 to 4. In formula (T1-1), Mb and y are synonymous with Mb and y in formula (T1), and the ideal range is also the same. [Chemical 17] In formula (T1-2), R is a base of a constituent unit represented by formula (Tx). [Chemical 18] In formula (Tx), n, o, and p are the average number of repeating units, n represents a number greater than 0 and less than 20, o and p independently represent numbers from 0 to 20, and 1.0 ≦ n + o + p ≦ 20.0. Ma represents a hydrocarbon group with 1 to 12 carbon atoms that can be substituted by halogen atoms. x represents an integer from 0 to 4. The constituent units (a), (b), and (c) are bonded by * and other groups, and the constituent units can also be bonded randomly.
[0022] In formula (Tx), n, o, and p refer to the average number of repeating units of all molecules in the resin. In formula (Tx), a sum of n, o, and p of 1.1 ≤ n + o + p is preferred, 1.2 ≤ n + o + p is even better, 1.5 ≤ n + o + p is even better, 2.0 ≤ n + o + p is even better, 2.5 ≤ n + o + p is even better, 3.0 ≤ n + o + p is even better, and 3.3 ≤ n + o + p is particularly good. Furthermore, in formula (Tx), a sum of n, o, and p of n + o + p ≤ 20.0 is preferred, n + o + p ≤ 10.0 is even better, n + o + p ≤ 8.0 is even better, n + o + p ≤ 7.0 is even better, and n + o + p ≤ 6.4 is even more ideal. The sum of n, o, and p can be calculated using the method described in the following embodiments. In formula (Tx), Ma and x are synonyms with Ma and x in formula (Txn), respectively, and their ideal ranges are also the same.
[0023] Furthermore, for the resin represented by formula (T1-1) (preferably the resin represented by formula (T1-1-2)), the parameter α calculated from formula (α) is preferably 0.55 to 1.00 and the parameter β calculated from formula (β) is preferably 0.20 to 3.00. With parameters α and β in the above ranges, the obtained cured material tends to have low dielectric properties (Dk and / or Df) and excellent heat resistance. [Number 1] Parameter α (α) Parameter β (β) The values in parentheses of formulas (α) and (β) represent the integral values between the corresponding chemical shift values of 1H-NMR.
[0024] Here, α represents the ratio of the constituent units (constituent unit (a) of formula (Tx)) having a dihydroindene skeleton in the resin represented by formula (T1-1), preferably the resin represented by formula (T1-1-2). More specifically, it is speculated that by adjusting the constituent units having a dihydroindene skeleton to a range that conforms to the above parameter α, the obtained resin molecules will have high rigidity and high glass transition temperature. Furthermore, molecules with high rigidity have lower mobility compared to molecules with low rigidity, so it is speculated that the dielectric tempering time is longer and the Df energy is lower. α can be increased by adjusting the raw material concentration, using a highly polar solvent, increasing the amount of catalyst, and increasing the reaction temperature when synthesizing the resin represented by formula (T1-1). On the other hand, β refers to the ratio of terminal double bonds in the resin represented by formula (T1-1) (preferably the resin represented by formula (T1-1-2)). More specifically, for example, it is speculated that other compounds (C) (especially thermosetting compounds) possess an increased number of crosslinking points of functional groups, making it easier to form a network during thermosetting, thus obtaining cured products with high glass transition temperatures and low Df. β can be increased by reducing the amount of catalyst, lowering the reaction temperature, and using low-polarity solvents when synthesizing the resin represented by formula (T1-1). When synthesizing the resin represented by formula (T1-1) (preferably the resin represented by formula (T1-1-2)), the parameters α and β of the resin represented by formula (T1-1) (preferably the resin represented by formula (T1-1-2)) can be adjusted by increasing the parameters α and β described above. Of course, parameters α and β can also be adjusted using methods other than those described above.
[0025] A parameter α of 0.57 or higher is preferred, 0.59 or higher is even better, 0.60 or higher is still better, 0.62 or higher is even better, and values of 0.65 or higher, 0.70 or higher, 0.75 or higher, and 0.80 or higher are also acceptable. By setting the parameter α above the aforementioned lower limit, the heat resistance of the obtained cured material tends to be better. Parameter α, in fact, tends to result in a cured material with low dielectric properties (Dk and / or Df) and excellent heat resistance, so a larger parameter α is preferred, but values of 0.95 or lower, 0.90 or lower, 0.85 or lower, 0.82 or lower, 0.80 or lower, 0.77 or lower, 0.75 or lower, and 0.74 or lower are also acceptable. A parameter β of 0.25 or higher is preferred, 0.30 or higher is even better, 0.35 or higher is even better, 0.40 or higher is even better, 0.43 or higher is even better, 0.50 or higher is even better, and values of 0.60, 0.65, 0.70, 0.77, 0.80, 0.90, and 0.95 or higher are also acceptable. By setting the parameter β to values above the aforementioned lower limits, the heat resistance of the hardened material is improved, and the heat resistance (Df) tends to decrease. A parameter β of 2.50 or lower is preferred, 2.00 or lower is even better, 1.50 or lower is even better, 1.30 or lower is even better, 1.20 or lower is even better, 1.10 or lower is even better, and values of 1.00, 0.95, 0.90, 0.85, 0.83, and 0.80 are also acceptable. When parameter β is below the aforementioned upper limit, the heat resistance of the hardened material tends to be improved and Df tends to be reduced.
[0026] The number average molecular weight (Mn) of the resin (A) converted from polystyrene by GPC (gel permeation chromatography) (details as described in the examples below) is preferably 400 or higher, more preferably 500 or higher, more preferably 550 or higher, more preferably 600 or higher, and ideally 650 or higher. By having the number average molecular weight above the aforementioned lower limit, the heat resistance of the obtained cured material is improved, and Df tends to decrease. Furthermore, the upper limit of the number average molecular weight (Mn) of the resin (A) converted from polystyrene by GPC (gel permeation chromatography) is preferably 3000 or lower, more preferably 2500 or lower, more preferably 2000 or lower, more preferably 1500 or lower, and even more preferably 1250 or lower. Depending on the application, it may also be 1000 or lower, or 800 or lower. When the number average molecular weight is below the aforementioned upper limit, the heat resistance of the cured material is improved, and the relative permittivity (Dk) and dielectric loss tangent (Df) tend to decrease. Furthermore, the weight average molecular weight (Mw) of resin (A) converted from polystyrene using GPC (details according to the method described in the examples below) is preferably 500 or higher, more preferably 800 or higher, more preferably 900 or higher, and ideally 1000 or higher. When the weight average molecular weight is above the aforementioned lower limit, the heat resistance of the cured material is improved, and Df tends to decrease. The upper limit of the weight-average molecular weight (Mw) of resin (A) converted from polystyrene using GPC (details according to the method described in the examples below) is preferably 6000 or less, more preferably 5000 or less, more preferably 4000 or less, more preferably 3000 or less, and more preferably 2800 or less. Depending on the application, it may also be 2500 or less, 2000 or less, or 1500 or less. The heat resistance of the cured material obtained by having a weight-average molecular weight below the aforementioned upper limit is improved, and there is a tendency to reduce the relative dielectric constant (Dk) and dielectric loss tangent (Df).
[0027] For resin (A), the ratio of weight average molecular weight to number average molecular weight, i.e., Mw / Mn, is preferably 1.1 to 3.0. It is more preferable that the Mw / Mn of resin (A) is 1.2 or higher, more preferably 1.3 or higher, more preferably 1.4 or higher, more preferably 1.5 or higher, and more preferably 1.6 or higher. Furthermore, it is more preferable that the Mw / Mn of resin (A) is 2.5 or lower, more preferably 2.4 or lower, and also acceptable that it is 2.3 or lower, 2.0 or lower, or 1.8 or lower. The weight average molecular weight and number average molecular weight were determined according to the methods described in the examples below.
[0028] In the resin composition of this embodiment, the content of resin (A) is preferably 5 parts by mass or more, more preferably 8 parts by mass or more, and 10 parts by mass or more, relative to 100 parts by mass of the resin solids in the resin composition. Depending on the application, 15 parts by mass or more, 20 parts by mass or more, and 25 parts by mass or more are also acceptable. When the content of resin (A) is above the aforementioned lower limit, there is a tendency to reduce the heat resistance (Df) of the obtained cured product. Furthermore, the upper limit of the content of resin (A) is preferably 70 parts by mass or less, more preferably 55 parts by mass or less, even more preferably 50 parts by mass or less, even more preferably 45 parts by mass or less, even more preferably 40 parts by mass or less, and especially preferably 35 parts by mass or less. When the content of resin (A) is below the aforementioned upper limit, there is a tendency to improve the moldability of the resin composition and the heat resistance of the obtained cured product. The resin composition of this embodiment may contain only one type of resin (A) or two or more types. When containing two or more types, the total amount is preferably within the range described above. The manufacturing method of resin (A) in this embodiment is not particularly limited, and resins obtained using known manufacturing methods can be used. Furthermore, the raw materials, reaction temperature, type of catalyst, amount of catalyst, reaction solvent, and concentration of raw materials used in the synthesis of resin (A) are not particularly limited, and can be appropriately selected or controlled according to the desired physical properties. In this embodiment, one example of the raw materials used in the synthesis of resin (A) may be m-bis(α-hydroxyisopropyl)benzene, p-bis(α-hydroxyisopropyl)benzene, 1,3-diisopropenylbenzene, and 1,4-diisopropenylbenzene. In this embodiment, the reaction temperature for synthesizing resin (A) is preferably 40°C or higher, more preferably 50°C or higher, more preferably 60°C or higher, and 70°C, 80°C, 90°C, 100°C, 110°C, and 120°C or higher are also acceptable. Reaching or exceeding the aforementioned lower limit tends to increase the reaction rate and the ratio of the dihydroindene skeleton (the constituent unit (a) of formula (Tx)), which is ideal. Furthermore, a reaction temperature of 180°C or lower is preferred, more preferably 150°C or lower, and even more preferably 140°C or lower. Reaching or below the aforementioned upper limit tends to effectively suppress the formation of byproducts. Also, the temperature can vary from start to finish without requiring the same reaction temperature. In this case, the average temperature of the reaction throughout the entire process is preferably within the above range. In this embodiment, the catalyst used for synthesizing resin (A) is not particularly limited, for example, an acid catalyst. Acid catalysts can be made from inorganic acids such as hydrochloric acid, sulfuric acid, and phosphoric acid; organic acids such as oxalic acid, benzenesulfonic acid, toluenesulfonic acid, methanesulfonic acid, and fluoromethanesulfonic acid; BF3 ether complexes and BF3 phenol complexes; Lewis acids such as aluminum chloride, zinc chloride, and indium chloride; solid acids such as activated clay, acidic clay, alumina silica, and zeolite; heteropolyhydrochloric acid; and strong acid ion exchange resins. When using a catalyst, its amount is, for example, 0.01 to 20.0 parts by mass relative to 100 parts by mass of the above-mentioned raw materials in resin (A).A single catalyst is typically used, but two or more catalysts may be used in combination. When used in combination, the total amount is preferably within the range described above. In this embodiment, the reaction solvent for synthesizing resin (A) is not particularly limited and may be used in combination with aromatic hydrocarbon solvents such as toluene, benzene, chlorobenzene, and xylene; halogenated hydrocarbon solvents such as dichloromethane and chloroform; aliphatic hydrocarbon solvents such as hexane and heptane; ester solvents such as ethyl acetate and propyl acetate; acetamide solvents such as dimethylformamide and dimethylacetamide; alcohol solvents; or ketone solvents. Water may also be added. Examples of alcohol solvents include methanol, ethanol, butanol, propanol, methyl propylene glycol, diethylene glycol ethyl ether, butyl propylene glycol, and propyl propylene glycol. Examples of ketone solvents include acetone, methyl ethyl ketone, diethyl ketone, methyl butyl ketone, and methyl isobutyl ketone. Other examples include tetrahydrofuran and dimethyl ether, but these are not limited to these. One example of a reaction solvent in this embodiment is one containing an aromatic hydrocarbon solvent. In this embodiment, the concentration of the aforementioned raw material during the synthesis of resin (A) is preferably 5% or more, more preferably 8% or more, more preferably 10% or more, and 12% or more, 15% or more, 17% or more, 20% or more, 22% or more, and 25% or more are also acceptable. By reaching the aforementioned lower limit or above, there is a tendency to increase the reaction rate and the ratio of the dihydroindene skeleton (the constituent unit (a) of formula (Tx)), which is preferable. Furthermore, the concentration of the aforementioned raw material is preferably 49% or less, and more preferably 40% or less. By reaching the aforementioned upper limit or below, there is a tendency to effectively suppress the formation of by-products. Also, the concentration does not need to be the same from the start to the end of the reaction; variations in concentration are acceptable.
[0029] <Polyphenylene ether compound (B) with carbon-carbon unsaturated double bonds at the ends> The resin composition of this embodiment contains a polyphenylene ether compound (B) with carbon-carbon unsaturated double bonds at the ends. In this embodiment, it is preferable that the polyphenylene ether compound (B) contains a polyphenylene ether compound (B2) with two or more carbon-carbon unsaturated double bonds. The polyphenylene ether compound (B) with a carbon-carbon unsaturated double bond at the end is preferably a polyphenylene ether compound with a group selected from the group consisting of vinylbenzyl (Rx-1), (meth)acrylate (Rx-2), and maleimide. A polyphenylene ether compound with a group represented by vinylbenzyl (Rx-1) and / or (meth)acrylate (Rx-2) is more preferred. A polyphenylene ether compound with two or more groups represented by vinylbenzyl (Rx-1) and / or (meth)acrylate (Rx-2) at the end is even more preferred. [Chemical 19] In formulas (Rx-1) and (Rx-2), R1, R2, and R3 each independently represent a hydrogen atom, alkyl, alkenyl, or alkynyl group. * represents the bonding site between the hydrogen atom and the oxygen atom. Mc each independently represents a hydrocarbon group having 1 to 12 carbon atoms. z represents an integer from 0 to 4. r represents an integer from 1 to 6.
[0030] By using such polyphenylene ether compounds, there is a tendency to more effectively improve the low dielectric properties (Dk and / or Df) and low water absorption of printed circuit boards, etc. In this embodiment, polyphenylene ether compounds with vinyl benzyl groups at the ends are particularly preferred. By having vinyl benzyl groups, there is a tendency to significantly improve the compatibility with resin (A). These matters will be explained in detail below.
[0031] A polyphenylene ether compound (B) having carbon-carbon unsaturated double bonds at the end (preferably a polyphenylene ether compound (B2) containing two or more carbon-carbon unsaturated double bonds), for example, a compound having a polyphenylene ether skeleton represented by the following formula (X1).
[0032] [Chemical 20] In formula (X1), R24, R25, R26, and R27 may be the same or different, representing alkyl, aryl, halogen, or hydrogen atoms with 6 or fewer carbon atoms.
[0033] A polyphenylene ether compound (B) having a carbon-carbon unsaturated double bond at the end (preferably a polyphenylene ether compound (B2) containing two or more carbon-carbon unsaturated double bonds), may also contain repeating units represented by formula (X2) and / or repeating units represented by formula (X3): [Chemical 21] In formula (X2), R28, R29, R30, R34, and R35 may be the same or different, representing alkyl or phenyl with 6 or fewer carbon atoms. R31, R32, and R33 may be the same or different, representing hydrogen atoms and alkyl or phenyl with 6 or fewer carbon atoms. [Chemical 22] In formula (X3), R36, R37, R38, R39, R40, R41, R42, and R43 may be the same or different, representing hydrogen atoms and alkyl or phenyl with 6 or fewer carbon atoms. -A- is a straight-chain, branched, or cyclic divalent hydrocarbon group with 20 or fewer carbon atoms.
[0034] The polyphenylene ether compound (B) having carbon-carbon unsaturated double bonds at the ends (preferably a polyphenylene ether compound (B2) containing two or more carbon-carbon unsaturated double bonds) is preferred. It is also preferable to be a modified polyphenylene ether compound (hereinafter sometimes referred to as "modified polyphenylene ether compound (g)") having one or more of the ends functionalized with vinylbenzyl groups (Rx-1), (meth)acrylate groups (Rx-2), or maleimide groups. Modified polyphenylene ether compounds having two or more groups at the ends selected from the group consisting of vinylbenzyl groups (Rx-1) and / or (meth)acrylate groups (Rx-2) are even more preferred. By using such a modified polyphenylene ether compound (g), the low dielectric properties (Dk and / or Df) of the cured resin composition are reduced, and the low water absorption and metal foil peel strength are improved. They can be used individually or in combination of two or more.
[0035] Modified polyphenylene ether compound (g), for example, a polyphenylene ether compound represented by formula (OP). [Chemical 23] In formula (OP), X represents an aromatic group, -(YO)n1- represents a polyphenylene ether structure, n1 represents an integer from 1 to 100, and n2 represents an integer from 1 to 4. Rx is a group represented by formula (Rx-1) or formula (Rx-2). [Chemical 24] In formulas (Rx-1) and (Rx-2), R1, R2, and R3 each independently represent a hydrogen atom, alkyl, alkenyl, or alkynyl group. * represents the bonding site between the group and the oxygen atom. Mc each independently represents a hydrocarbon group with 1 to 12 carbon atoms. z represents an integer from 0 to 4. r represents an integer from 1 to 6.
[0036] When n1 and / or n2 are integers greater than 2, the n1 constituent units (YO) and / or n2 constituent units can be the same or different. It is ideal for n2 to be greater than 2, and even better if it is 2.
[0037] In formulas (Rx-1) and (Rx-2), R1, R2, and R3 each independently represent a hydrogen atom, an alkyl group, an alkenyl group, or an alkynyl group. Ideally, R1 should be a hydrogen atom or an alkyl group, with a hydrogen atom or a methyl group being more preferred, and a hydrogen atom being even more preferred. Ideally, R2 and R3 should each be an alkyl group or an alkyl group, with a hydrogen atom or a methyl group being more preferred, and a hydrogen atom being even more preferred. Regarding the number of carbon atoms in the alkyl, alkenyl, or alkynyl groups of R1, R2, and R3, 5 or less is preferred, and 3 or less is even more preferred.
[0038] In formula (Rx-1), r represents an integer from 1 to 6, with integers from 1 to 5 being better, integers from 1 to 4 being even better, integers from 1 to 3 being even better, 1 or 2 being even better, and 1 being the most ideal.
[0039] In formula (Rx-1), Mc independently represents a hydrocarbon group having 1 to 12 carbon atoms, preferably a hydrocarbon group having 1 to 10 carbon atoms, and even more preferably a straight-chain or branched alkyl group having 1 to 10 carbon atoms. Methyl, ethyl, isopropyl, isobutyl, tributyl, pentyl, octyl, or nonyl are preferred, and methyl, ethyl, isopropyl, isobutyl, or tributyl are even more ideal. In formula (Rx-1), z represents an integer from 0 to 4, preferably an integer from 0 to 3, even more preferably an integer from 0 to 2, even more preferably 0 or 1, and even more ideally 0.
[0040] A specific example of the group represented by formula (Rx-1) is vinylbenzyl, and a specific example of the group represented by formula (Rx-2) is (meth)acrylyl. It is preferable that Rx is a group represented by formula (Rx-1).
[0041] Modified polyphenylene ether compound (g), for example, a polyphenylene ether compound represented by formula (OP-1). [Chemical 25] In formula (OP-1), X represents an aromatic group, -(YO)n 2- represents a polyphenylene ether structure, R1, R2, and R3 each independently represent a hydrogen atom, alkyl, alkenyl, or alkynyl group, n1 represents an integer from 1 to 6, n2 represents an integer from 1 to 100, and n3 represents an integer from 1 to 4. When n2 and / or n3 are integers of 2 or more, the n2 constituent units (YO) and / or n3 constituent units may be the same or different. It is ideal for n3 to be 2 or more, and more preferably 2.
[0042] In this embodiment, the modified polyphenylene ether compound (g) is preferably represented by formula (OP-2), and more preferably by formula (OP-2-2). [Chemical 26][Chemical 27] Here, -(OXO)- is preferably represented by formula (OP-3) and / or formula (OP-4). [Chemical 28] In formula (OP-3), R4, R5, R6, R10, and R11 may be the same or different, and are alkyl or phenyl with 6 or fewer carbon atoms. R7, R8, and R9 may be the same or different, and are hydrogen atoms, alkyl or phenyl with 6 or fewer carbon atoms. [Chemical 29] In formula (OP-4), R12, R13, R14, R15, R16, R17, R18, and R19 may be the same or different, and are hydrogen atoms, alkyl or phenyl with 6 or fewer carbon atoms. -A- is a straight-chain, branched, or cyclic divalent hydrocarbon group with 20 or fewer carbon atoms.
[0043] Furthermore, -(YO)- is preferably represented by formula (OP-5). [Chemical 30] In formula (OP-5), R20 and R21 may be the same or different, and are alkyl or phenyl with 6 or fewer carbon atoms. R22 and R23 may be the same or different, and are hydrogen atoms, alkyl or phenyl with 6 or fewer carbon atoms. In particular, by having R20 and R21 each independently as a group having one or more methyl and / or cyclohexyl groups, the rigidity of the obtained resin molecule is improved. Molecules with high rigidity have lower mobility than molecules with low rigidity, so the dielectric relaxation time is increased and the low dielectric properties (Dk and / or Df) are improved, which is preferred. An example of formula (OP-5) is the following structure. [Chemical 31] For polyphenylene ether compounds having the above structure, please refer to the description in Japanese Patent Application Publication No. 2019-194312, the contents of which are incorporated herein by reference.
[0044] In formula (OP-2), a and b each independently represent an integer from 0 to 100, and at least one of a and b is an integer from 1 to 100. It is preferable that a and b are each independent integers from 0 to 50, more preferably integers from 1 to 30, and more preferably integers from 1 to 10. When a and / or b are integers of 2 or more, the two or more -(YO)- can each be arranged in one structural arrangement, or the two or more structures can be arranged in a block or random arrangement. Furthermore, when there are compounds represented by multiple formulas (OP-2), it is preferable that the average value of a is 1 < a < 10, and the average value of b is 1 < b < 10.
[0045] The -A- in formula (OP-4) can be, for example, methylene, ethylene, 1-methylethylene, 1,1-propylene, 1,4-epoxyphenylbis(1-methylethylene), 1,3-epoxyphenylbis(1-methylethylene), cyclohexene, phenylmethylene, naphthylmethylene, 1-phenylethylene, and other divalent organogroups, but is not limited to these.
[0046] Rx and Rx in formula (OP) are synonymous, and the ideal range is also the same.
[0047] Among the compounds represented by formula (OP-2) above, it is preferable that R4, R5, R6, R10, R11, R20, and R21 are alkyl groups with 3 or fewer carbon atoms, and that R7, R8, R9, R12, R13, R14, R15, R16, R17, R18, R19, R22, and R23 are alkyl polyphenylene ether compounds with hydrogen atoms or 3 or fewer carbon atoms. In particular, it is preferable that -(OXO)- represented by formula (OP-3) or formula (OP-4) is formula (OP-9), formula (OP-10), and / or formula (OP-11), and that -(YO)- represented by formula (OP-5) is formula (OP-12) or formula (OP-13).
[0048] When a and / or b are integers of 2 or more, each of the two or more -(YO)- can be independently a structure composed of two or more of the formulas (OP-12) and / or (OP-13), or a structure composed of segments or random arrangements of the formulas (OP-12) and (OP-13).
[0049] [Chemical 32][Chemical 33] In formula (OP-10), R 44, R 45, R 46, and R 47 may be the same or different, and may be hydrogen atoms or methyl groups. -B- is a straight-chain, branched, or cyclic divalent hydrocarbon group with 20 or fewer carbon atoms. Specific examples of -B- may be the same as those of -A- in formula (OP-4). [Chemical 34] In formula (OP-11), -B- is a straight-chain, branched, or cyclic divalent hydrocarbon group with 20 or fewer carbon atoms. Specific examples of -B- may be the same as those of -A- in formula (OP-4). [Chemical 35][Chemical 36]
[0050] The modified polyphenylene ether compound (g) used in this embodiment is preferably a compound represented by formula (OP-14) and / or a compound represented by formula (OP-15). [Chemical 37] In formula (OP-14), a and b each independently represent an integer from 0 to 100, and at least one of a and b is an integer from 1 to 100. a and b in formula (OP-14) are each independently synonymous with a and b in formula (OP-2), and the ideal range is also the same. [Chemical 38] In formula (OP-15), a and b each independently represent an integer from 0 to 100, and at least one of a and b is an integer from 1 to 100. a and b in formula (OP-15) are each independently synonymous with a and b in formula (OP-2), and the ideal range is also the same.
[0051] The number average molecular weight (Mn) of a polyphenylene ether compound (B) with carbon-carbon unsaturated double bonds at the ends (preferably a polyphenylene ether compound (B2) containing two or more carbon-carbon unsaturated double bonds, and more preferably a modified polyphenylene ether compound (g)) measured by GPC (gel permeation chromatography) using polystyrene conversion (details as described in the examples below), is preferably 500 or higher, 800 or higher, and 3,000 or lower. With a number average molecular weight of 500 or higher, the stickiness of the resin composition of this embodiment when formed into a film is more suppressed. With a number average molecular weight of 3,000 or lower, the solubility in solvents is more improved. Furthermore, the weight-average molecular weight (Mw) of the polyphenylene ether compound (B) with carbon-carbon unsaturated double bonds at the ends (preferably a polyphenylene ether compound (B2) containing two or more carbon-carbon unsaturated double bonds, and more preferably a modified polyphenylene ether compound (g)) measured by GPC (details according to the method described in the examples below) is preferably 800 to 6000, and more preferably 800 to 5000. By setting the aforementioned lower limit or above, the relative permittivity (Dk) and dielectric loss tangent (Df) of the cured resin composition tend to be lower, and by setting the aforementioned upper limit or below, the resin composition tends to have improved solvent solubility, low viscosity, and formability when making the varnishes described later. Furthermore, in the case of modified polyphenylene ether compounds (g), the equivalent amount of terminal carbon-carbon unsaturated double bonds is preferably 400-5000 g per carbon-carbon unsaturated double bond, and more preferably 400-2500 g. By exceeding the aforementioned lower limit, the relative permittivity (Dk) and dielectric loss tangent (Df) of the cured resin composition tend to become lower. By falling below the aforementioned upper limit, the resin composition tends to have improved solvent solubility, low viscosity, and formability.
[0052] In the resin composition of this embodiment, the lower limit of the content of polyphenylene ether compound (B) with carbon-carbon unsaturated double bonds at the ends (preferably polyphenylene ether compound (B2) containing two or more carbon-carbon unsaturated double bonds) is 10 parts by mass or more, preferably 50 parts by mass or more, more preferably 100 parts by mass or more, more preferably 150 parts by mass or more, and also preferably 180 parts by mass or more, relative to 100 parts by mass or more. By reaching the aforementioned lower limit or above, the formability of the resin composition, the low water absorption of the obtained cured product, and the low dielectric properties (Dk and / or Df) tend to be further improved. Furthermore, the upper limit of the content of polyphenylene ether compound (B) with carbon-carbon unsaturated double bonds at the ends (preferably polyphenylene ether compound (B2) containing two or more carbon-carbon unsaturated double bonds) is preferably 300 parts by mass or less, 280 parts by mass or less, 250 parts by mass or less, or 220 parts by mass or less, relative to 100 parts by mass of resin (A). By being below the aforementioned upper limit, the cured material tends to have improved low dielectric properties (Dk and / or Df), heat resistance, and chemical resistance.
[0053] In this embodiment, the total content of resin (A) and polyphenylene ether compound (B) relative to 100 parts by mass of resin solids in the resin composition is preferably 40 parts by mass or more, more preferably 45 parts by mass or more, more preferably 50 parts by mass or more, and 55 parts by mass or more is also acceptable. When the total content of resin (A) and polyphenylene ether compound (B) is at or above the aforementioned lower limit, the resulting cured product tends to have improved low water absorption and low dielectric properties (Dk and / or Df). Furthermore, the total content of resin (A) and polyphenylene ether compound (B) relative to 100 parts by mass of resin solids in the resin composition is preferably 80 parts by mass or less. When the total content of resin (A) and polyphenylene ether compound (B) is at or below the aforementioned upper limit, the resin composition tends to have excellent balance in terms of formability, the resulting cured product's low dielectric properties (Dk and / or Df), heat resistance, and chemical resistance.
[0054] In this embodiment, relative to 100 parts by mass of the total resin (A) and polyphenylene ether compound (B), a mass ratio of resin (A) of 10 parts by mass or more is preferred, 15 parts by mass or more is more preferred, 20 parts by mass or more is more preferred, 25 parts by mass or more is even more preferred, and 30 parts by mass or more is ideal. When the aforementioned mass ratio is at or above the lower limit, the low dielectric properties (Dk and / or Df) of the obtained cured product tend to be further improved. Furthermore, relative to 100 parts by mass of the total resin (A) and polyphenylene ether compound (B), a mass ratio of resin (A) of 50 parts by mass or less is preferred, 45 parts by mass or less is more preferred, 40 parts by mass or less is even more preferred, and 38 parts by mass or less is even more ideal. When the aforementioned mass ratio is at or below the upper limit, the formability of the resin composition and the low dielectric properties (Dk and / or Df) of the obtained cured product tend to be further improved.
[0055] In the resin composition of this embodiment, the lower limit of the content of polyphenylene ether compound (B) with terminal carbon-carbon unsaturated double bonds (preferably polyphenylene ether compound (B2) containing two or more carbon-carbon unsaturated double bonds) is preferably 30 parts by mass or more, and more preferably 35 parts by mass or more, relative to 100 parts by mass of resin solids in the resin composition. By achieving the aforementioned lower limit or above, the cured product tends to have improved low water absorption and low dielectric properties (Dk and / or Df). Furthermore, the upper limit of the content of polyphenylene ether compound (B) with terminal carbon-carbon unsaturated double bonds (preferably polyphenylene ether compound (B2) containing two or more carbon-carbon unsaturated double bonds) is preferably 75 parts by mass or less, more preferably 70 parts by mass or less, and also 65 parts by mass or less, or even 60 parts by mass or less, relative to 100 parts by mass of resin solids in the resin composition. By setting the value below the aforementioned upper limit, the heat resistance and chemical resistance of the obtained cured material tend to be further improved. The resin composition in this embodiment may contain only one type of polyphenylene ether compound (B) with a terminal carbon-carbon unsaturated double bond, or it may contain two or more types. When containing two or more types, the total amount within the aforementioned range is preferred.
[0056] <Polymer having constituent units represented by formula (V)> The resin composition of this embodiment contains a polymer having constituent units represented by formula (V). By using a polymer containing constituent units represented by formula (V), a resin composition that provides excellent low dielectric properties (Dk and / or Df) can be obtained. [Chemical 39] In formula (V), Ar represents an aromatic hydrocarbon linker. * indicates a bond position.
[0057] The aromatic hydrocarbon linking group can be a group consisting solely of an aromatic hydrocarbon that may also have substituents, or it can be a group consisting of an aromatic hydrocarbon that may also have substituents combined with other linking groups. It is preferable that the group consists solely of an aromatic hydrocarbon that may also have substituents. Furthermore, aromatic hydrocarbons may also possess substituents, such as substituent Z (e.g., alkyl groups having 1 to 6 carbon atoms, alkenyl groups having 2 to 6 carbon atoms, alkoxy groups having 2 to 6 carbon atoms, hydroxyl groups, amino groups, carboxyl groups, halogen atoms, etc.). It is preferable that the aforementioned aromatic hydrocarbons do not have substituents. The aromatic hydrocarbon linking group is usually a divalent linking group.
[0058] The aromatic hydrocarbon linking group, specifically, may also have substituents such as phenyl, naphthyl, anthracenediyl, phenanthrenediyl, biphenyldiyl, and fenandrolone, among which phenyl may also have substituents, preferably phenyl. Substituents such as the above-mentioned substituent Z, and preferably the above-mentioned phenyl group, are unsubstituents.
[0059] The constituent unit represented by formula (V) preferably includes at least one of the constituent units represented by formula (V1), formula (V2), and formula (V3). Furthermore, * in the following formulas indicates the bond position. Also, the constituent units represented by formulas (V1) to (V3) are sometimes collectively referred to as "constituent unit (a)".
[0060] [Chemical 40] In formulas (V1) to (V3), L1 is an aromatic hydrocarbon linker (preferably with 6 to 22 carbon atoms, more preferably 6 to 18, and even more preferably 6 to 10). Specifically, for example, substituents such as phenyl, naphthyl, anthracene, phenanthrene, biphenyl, and fenediyl may also be used, among which phenyl may also be used, which is preferred. Substituents such as the aforementioned substituent Z, and the aforementioned phenyl groups are preferably unsubstituented. As for the compound forming the constituent unit (a), a divinyl aromatic compound is preferred, such as: divinylbenzene, bis(1-methylvinyl)benzene, divinylnaphthalene, divinylanthracene, divinylbiphenyl, divinylphenanthrene, etc. Among them, divinylbenzene is particularly preferred. One of these divinyl aromatic compounds may also be used, and two or more may be used as needed.
[0061] The polymer having the constituent unit represented by formula (V) as described above can be a homopolymer of constituent unit (a) or a copolymer of constituent units from other monomers. When the polymer having the constituent unit represented by formula (V) is a copolymer, for its copolymerization ratio, it is preferable that constituent unit (a) is 3 mol% or more, more preferably 5 mol% or more, more preferably 10 mol% or more, and 15 mol% or more is also acceptable. The upper limit is preferably 90 mol% or less, more preferably 85 mol% or less, more preferably 80 mol% or less, even more preferably 70 mol% or less, more preferably 60 mol% or less, even more preferably 50 mol% or less, more preferably 40 mol% or less, even more preferably 30 mol% or less, and 25 mol% or less or 20 mol% or less is also acceptable.
[0062] Constituents derived from other monomers, such as constituents (b) derived from an aromatic compound having one vinyl group (monovinyl aromatic compound).
[0063] The constituent unit (b) from the monovinyl aromatic compound is preferably a constituent unit represented by the following formula (V4).
[0064] [Chemical 41] In formula (V4), L2 is an aromatic hydrocarbon linking group, ideally exemplified by the example of L1 described above. RV1 is a hydrogen atom or a hydrocarbon group having 1 to 12 carbon atoms (preferably an alkyl group). When RV1 is a hydrocarbon group, 1 to 6 carbon atoms are preferred, and 1 to 3 carbon atoms are even more preferred. RV1 and L2 may also have the substituent Z described above.
[0065] When the polymer having the constituent unit represented by formula (V) is a copolymer containing the constituent unit (b) from a monovinyl aromatic compound, examples of monovinyl aromatic compounds include vinyl aromatic compounds such as styrene, vinylnaphthalene, and vinyl biphenyl; nucleoalkyl-substituted vinyl aromatic compounds such as o-methylstyrene, m-methylstyrene, p-methylstyrene, o-, p-dimethylstyrene, o-ethylvinylbenzene, m-ethylvinylbenzene, p-ethylvinylbenzene, methylvinylbiphenyl, and ethylvinylbiphenyl. The monovinyl aromatic compounds illustrated here may also appropriately have the aforementioned substituent Z. Furthermore, one or more of these monovinyl aromatic compounds may be used.
[0066] When the polymer having the constituent unit represented by formula (V) is a copolymer containing constituent unit (b), the copolymerization ratio of constituent unit (b) is preferably 10 mol% or more, more preferably 15 mol% or more, and 20 mol% or more, 30 mol% or more, 40 mol% or more, 50 mol% or more, 60 mol% or more, 70 mol% or more, and 75 mol% or more. The upper limit is preferably 98 mol% or less, more preferably 90 mol% or less, and even more preferably 85 mol% or less.
[0067] Polymers having the constituent units represented by formula (V) may also have other constituent units besides constituent units (a) and (b). Other constituent units include, for example, constituent units (c) from cyclic olefin compounds. Cyclic olefin compounds include, for example, hydrocarbons having double bonds within their ring structures. Specifically, monocyclic cyclic olefins such as cyclobutene, cyclopentene, cyclohexene, and cyclooctene; in addition, compounds having a norunten ring structure such as norcamphene and dicyclopentadiene; and aromatic cyclic condensation compounds such as indene and vinylnaphthalene. Examples of norunten compounds are described in paragraphs 0037 to 0043 of Japanese Patent Application Publication No. 2018-39995, and such content is incorporated herein by reference. Furthermore, the cyclic olefin compounds illustrated here may also have the aforementioned substituent Z.
[0068] When the polymer having the constituent unit represented by formula (V) is a copolymer containing the constituent unit (c), the copolymerization ratio of the constituent unit (c) is preferably 10 mol% or more, more preferably 20 mol% or more, and even more preferably 30 mol% or more. The upper limit is preferably 90 mol% or less, more preferably 80 mol% or less, more preferably 70 mol% or less, and 50 mol% or less is also acceptable, as is 30 mol% or less.
[0069] The polymer having the constituent units represented by formula (V) may also include constituent units (d) from different polymerizable compounds (hereinafter also referred to as other polymerizable compounds). Other polymerizable compounds (monomers) include, for example, compounds containing three vinyl groups. Specifically, 1,3,5-trivinylbenzene, 1,3,5-trivinylnaphthalene, 1,2,4-trivinylcyclohexane. Or, for example, ethylene glycol diacrylate, butadiene, etc. The copolymerization ratio of constituent units (d) from other polymerizable compounds is preferably 30 mol% or less, more preferably 20 mol% or less, and even more preferably 10 mol% or less.
[0070] In one embodiment of the polymer having the constituent unit represented by formula (V), the constituent unit (a) is necessary, for example, a polymer containing at least one of the constituent units (b) to (d). Furthermore, for example, the total percentage of constituent units (a) to (d) is 95 mol% or more, and further 98 mol% or more of all constituent units. In another embodiment of the polymer having the constituent unit represented by formula (V), it is preferable that the constituent unit (a) is necessary, and that the percentage of constituent units containing aromatic rings among all constituent units excluding the terminal units is 90 mol% or more, more preferably 95 mol% or more, and 100 mol% is also acceptable. Furthermore, when calculating the mol% of all constituent units, one constituent unit refers to one molecule of a monomer (e.g., a divinyl aromatic compound, a monovinyl aromatic compound, etc.) used in the manufacture of the polymer having the constituent unit represented by formula (V).
[0071] The manufacturing method of the polymer having the constituent unit represented by formula (V) is not particularly limited, and can be carried out by conventional methods, such as polymerizing a raw material containing a divinyl aromatic compound (if necessary, a monovinyl aromatic compound, a cycloolefin compound, etc. may coexist) in the presence of a Lewis acid catalyst. The Lewis acid catalyst may be a metal fluoride such as boron trifluoride or a complex thereof.
[0072] The structure of the chain ends of polymers having constituent units represented by formula (V) is not particularly limited. For example, for groups derived from the aforementioned divinyl aromatic compounds, the structure of formula (E1) can be adopted. Furthermore, L1 in formula (E1) is defined in the same way as in formula (V1) above. * represents the bond position. *-CH=CH-L1-CH=CH2 (E1)
[0073] When the group from a monovinyl aromatic compound becomes the chain terminus, the structure of formula (E2) can be adopted. L2 and RV1 in this formula have the same meaning as defined in formula (V4). * represents the bond position. *-CH=CH-L2-RV1(E2)
[0074] The molecular weight of the polymer having the constituent unit represented by formula (V), based on the number average molecular weight Mn, is preferably 300 or more, more preferably 500 or more, more preferably 1,000 or more, and more preferably 1,500 or more. The upper limit is preferably 130,000 or less, more preferably 120,000 or less, more preferably 110,000 or less, and even more preferably 100,000 or less. The molecular weight of the polymer having the constituent unit represented by formula (V), based on the weight average molecular weight Mw, is preferably 3,000 or more, more preferably 5,000 or more, and even more preferably 10,000 or more. By having the aforementioned lower limit or above, the polymer having the constituent unit represented by formula (V) exhibits excellent low dielectric properties, especially Df and dielectric properties after moisture absorption, which can be effectively utilized in the cured form of the resin composition. The upper limit is preferably below 130,000, more preferably below 100,000, more preferably below 80,000, and even more ideally below 50,000. By being below the aforementioned upper limit, there is a tendency to cause poor filling when the prepreg or resin sheet is laminated on the circuit forming substrate. The monodispersity (Mw / Mn), expressed as the ratio of weight average molecular weight Mw to number average molecular weight Mn, is preferably below 100, more preferably below 50, and even more preferably below 20. The lower limit is practically 1.1 or more, 5 or more is preferred, 7 or more is preferred, and 10 or more is even more preferred. The above Mw and Mn can be measured according to the description of the embodiments described later. When the resin composition of this embodiment contains two or more polymers having constituent units represented by formula (V), the Mw, Mn, and Mw / Mn of the mixture should preferably conform to the above ranges.
[0075] The vinyl equivalent of the polymer having the constituent unit represented by formula (V) is preferably 200 g / eq. or more, more preferably 230 g / eq. or more, and even more preferably 250 g / eq. or more. Furthermore, the vinyl equivalent is preferably 1200 g / eq. or less, more preferably 1000 g / eq. or less, and 800 g / eq. or less, 600 g / eq. or less, 400 g / eq. or less, and 300 g / eq. or less. By achieving the aforementioned lower limit or above, the storage stability of the resin composition is improved, and the flowability of the resin composition tends to increase. Therefore, the formability is improved, and porosity is less likely to occur during the formation of prepregs, etc., leading to a tendency to obtain printed circuit boards with higher reliability. On the other hand, by achieving the aforementioned upper limit or below, the heat resistance of the obtained cured material tends to improve.
[0076] In this specification, polymers having constituent units represented by formula (V) can refer to the compounds and their synthesis reaction conditions described in paragraphs 0029 to 0058 of International Patent Publication No. 2017 / 115813, the compounds and their synthesis reaction conditions described in paragraphs 0013 to 0058 of Japanese Patent Application Publication No. 2018-039995, and the compounds described in paragraphs 0008 to 0043 of Japanese Patent Application Publication No. 2018-168347. Compounds and their synthesis reaction conditions, etc., as well as compounds and their synthesis reaction conditions described in paragraphs 0014 to 0042 of Japanese Patent Application Publication No. 2006-070136, compounds and their synthesis reaction conditions described in paragraphs 0014 to 0061 of Japanese Patent Application Publication No. 2006-089683, and compounds and their synthesis reaction conditions described in paragraphs 0008 to 0036 of Japanese Patent Application Publication No. 2008-248001, are included in this specification.
[0077] The lower limit of the content of the polymer having the constituent unit represented by formula (V) is preferably 10 parts by mass or more, 20 parts by mass or more, 40 parts by mass or more, 60 parts by mass or more, and 80 parts by mass or more, relative to 100 parts by mass of resin (A). On the other hand, the upper limit of the content of the polymer having the constituent unit represented by formula (V) is preferably 300 parts by mass or less, 280 parts by mass or less, 260 parts by mass or less, 240 parts by mass or less, and 220 parts by mass or less, relative to 100 parts by mass of resin (A). With the content within the above range, there is a tendency for excellent balance in the formability of the resin composition, the low dielectric properties (Dk and / or Df) of the obtained cured product, heat resistance, chemical resistance, etc.
[0078] The lower limit value of the polymer content of the constituent unit represented by formula (V) is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, more preferably 15 parts by mass or more, and more preferably 20 parts by mass or more when the resin solids content in the resin composition is 100 parts by mass. On the other hand, the upper limit value of the polymer content of the constituent unit represented by formula (V) is preferably 60 parts by mass or less, more preferably 55 parts by mass or less, more preferably 50 parts by mass or less, and more preferably 45 parts by mass or less when the resin solids content in the resin composition is 100 parts by mass.
[0079] In this embodiment, relative to 100 parts by mass of the resin (A) and the polymer having the constituent unit represented by formula (V), the mass ratio of resin (A) is preferably 10 parts by mass or more, more preferably 15 parts by mass or more, more preferably 20 parts by mass or more, and even more preferably 25 parts by mass or more. By being at or above the aforementioned lower limit, the low dielectric properties (Dk and / or Df) tend to be further improved. Furthermore, relative to 100 parts by mass of the resin (A) and the polymer having the constituent unit represented by formula (V), the mass ratio of resin (A) is preferably 70 parts by mass or less, and 65 parts by mass or less is also acceptable. By being at or below the aforementioned upper limit, the heat resistance tends to be further improved. The polymer having the constituent unit represented by formula (V) may contain only one type or may contain two or more types in the resin composition. When two or more types are contained, the total amount within the above range is preferred.
[0080] In this embodiment, it is illustrated that the total amount of resin (A), polyphenylene ether compound (B), and polymer having a constituent unit represented by formula (V) accounts for more than 90 parts by mass of the resin composition in 100 parts by mass of the resin solid component.
[0081] <Other Compounds (C)> The resin composition of this embodiment preferably contains other compounds (C) besides the resin (A), polyphenylene ether compound (B), and polymers having constituent units represented by formula (V) (preferably other curing compounds and / or plastic compounds, more preferably other thermosetting compounds and / or thermoplastic compounds, and even more preferably other thermosetting compounds). Other compounds (C) preferably contain compounds selected from maleimide compounds, cyanate compounds, epoxy compounds, phenolic compounds, compounds containing (methyl)allyl groups (e.g., alkenyl nadic imidin compounds), oxetane resins, benzo[a]benzene compounds, arylcyclobutene resins, polyamide resins, polyimide resins, perfluoroethylene ether resins, styrene compounds other than the aforementioned polyphenylene ether compound (B) with carbon-carbon unsaturated double bonds at the ends, and the aforementioned resin (A) with a dihydroindene skeleton. It is preferable to contain one or more of the following: compounds having an isopropylene group, polyphenylene ether compounds (B) with carbon-carbon unsaturated double bonds at the ends, polyfunctional (meth)acrylate compounds, elastomers, and petroleum resins. It is even more preferable to contain at least one of the following: compounds selected from maleimide compounds, cyanate ester compounds, epoxy compounds, phenolic compounds, compounds containing (meth)allyl groups (e.g., alkenyl nadicliimide compounds), oxetane resins, and benzo[a]pyrene compounds. By containing such components, the desired performance of the printed circuit board can be more effectively achieved.
[0082] When the resin composition of this embodiment contains other compounds (C), their content (total amount) relative to 100 parts by mass of the resin solids is preferably 1 part by mass or more, more preferably 10 parts by mass or more, more preferably 15 parts by mass or more, more preferably 20 parts by mass or more, and more preferably 30 parts by mass or more. By reaching the aforementioned lower limit or above, heat resistance, plating adhesion, and low thermal expansion tend to be further improved. Furthermore, the upper limit of the content of other compounds (C) (preferably other curing compounds and / or plastic compounds, more preferably other thermosetting compounds and / or thermoplastic compounds, and even more preferably other thermosetting compounds) relative to 100 parts by mass of the resin solids is preferably 50 parts by mass or less, more preferably 45 parts by mass or less, and more preferably 40 parts by mass or less. By reaching the aforementioned upper limit or below, low dielectric properties (Dk and / or Df) and low water absorption tend to be further improved. The resin composition of this embodiment may contain only one other compound (C), or it may contain two or more. When it contains two or more compounds, the total amount is preferably within the range described above.
[0083] <<Maleimimine Compound>> The resin composition of this embodiment may also contain a maleimimine compound. The maleimimine compound is not particularly limited as long as it contains one or more maleimimine groups in its molecule (preferably 2 to 12, more preferably 2 to 6, more preferably 2 to 4, preferably 2 or 3), and can be widely used in the field of printed circuit boards. In this embodiment, the maleimine compound preferably contains one or more compounds selected from the group consisting of compounds represented by formula (M0), formula (M1), formula (M2), formula (M3), formula (M4), formula (M5), maleimine compound (M6), and maleimine compound (M7), and is preferably contained in compounds selected from formula (M0), formula (M1), formula (M3), formula (M4), and formula (M5). It is more preferable to contain one or more compounds from the group consisting of maleimide compounds (M6), and it is even more preferable to contain one or more compounds from the group consisting of compounds represented by formula (M1), formula (M3), formula (M4), and formula (M5), it is even more preferable to contain one or more compounds from the group consisting of compounds represented by formula (M1), formula (M3), and formula (M5), it is even more preferable to contain compounds represented by formula (M1) and / or formula (M3), and it is more ideal to contain compounds represented by formula (M1). If these maleimide compounds are used in printed circuit board materials (e.g., metal-clad laminates), they can impart excellent heat resistance.
[0084] [Chemical 42] In formula (M0), R 51 each independently represents a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, or a phenyl group; R 52 each independently represents a hydrogen atom or a methyl group; and n 1 represents an integer greater than or equal to 1. R 51 is preferably selected from the group consisting of hydrogen atoms, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tributyl, n-pentyl, and phenyl, with hydrogen atoms and / or methyl being more preferred, and hydrogen atoms being even more preferred. R 52 is preferably methyl. n 1 is ideally an integer from 1 to 10, more preferably an integer from 1 to 5, more preferably an integer from 1 to 3, 1 or 2 is even more preferred, and 1 is even more preferred. Specifically, the following compounds can be listed as ideal examples of formula (M0). [Chemical 43] In the above formula, R 8 each independently represents a hydrogen atom, a methyl group, or an ethyl group, with methyl being preferred.
[0085] The compound represented by formula (M0) may be a single compound or a mixture of two or more compounds. Examples of mixtures include mixtures of compounds with different n1, mixtures of compounds with different types of substituents in R51 and / or R52, mixtures of compounds with different bonding positions (meta, para, or ortho) of maleimine group and oxygen atom relative to the benzene ring, and mixtures of compounds formed by combining two or more of the aforementioned different positions. The same applies to compounds represented by formulas (M1) to (M6) below. [Chemical 44] In formula (M1), RM1, RM2, RM3, and RM4 each independently represent a hydrogen atom or an organic group. RM5 and RM6 each independently represent a hydrogen atom or an alkyl group. ArM represents a divalent aromatic group. A is a 4- to 6-membered alicyclic group. RM7 and RM8 each independently represent an alkyl group. mx is 1 or 2, and lx is 0 or 1. RM9 and RM10 each independently represent a hydrogen atom or an alkyl group. RM11, RM12, RM13, and RM14 each independently represent a hydrogen atom or an organic group. RM15 each independently represents an alkyl group with 1 to 10 carbon atoms, an alkoxy group with 1 to 10 carbon atoms, an alkylthio group with 1 to 10 carbon atoms, a cycloalkyl group with 3 to 10 carbon atoms, an aryl group with 6 to 10 carbon atoms, an aryloxy group with 6 to 10 carbon atoms, an arylthio group with 6 to 10 carbon atoms, a halogen atom, a hydroxyl group, or a mercapto group. px represents an integer from 0 to 3. nx represents an integer from 1 to 20.
[0086] In the formula, RM1, RM2, RM3, and RM4 each independently represent a hydrogen atom or an organic group. It is preferred that the organic group is alkyl, more preferably alkyl with 1 to 12 carbon atoms, and ideally alkyl with 1 to 6 carbon atoms, with methyl, ethyl, propyl, and butyl being even more desirable, among which methyl is particularly preferred. RM1 and RM3 are each preferably alkyl, while RM2 and RM4 are preferably hydrogen atoms. RM5 and RM6 each independently represent a hydrogen atom or an alkyl group, with alkyl being preferred. It is preferred that the alkyl group is alkyl with 1 to 12 carbon atoms, more preferably alkyl with 1 to 6 carbon atoms, with methyl, ethyl, propyl, and butyl being even more desirable, among which methyl is particularly preferred. ArM represents a divalent aromatic group, preferably phenyl, naphthyl, phenanthrene, or anthracene, more preferably phenyl, and even more preferably m-phenyl. Ar M may also have substituents, with alkyl groups being preferred, especially alkyl groups with 1 to 12 carbon atoms, and even more so alkyl groups with 1 to 6 carbon atoms. Methyl, ethyl, propyl, and butyl groups are preferred, with methyl being the most desirable. However, Ar M is preferred to be unsubstituted. A is a 4- to 6-membered alicyclic group, with a 5-membered alicyclic group (preferably fused with a benzene ring to form a dihydroindene ring) being more desirable. RM7 and RM8 are each independently alkyl groups, with alkyl groups with 1 to 6 carbon atoms being preferred, and alkyl groups with 1 to 3 carbon atoms being more desirable, with methyl being the most desirable. mx is 1 or 2, with 2 being preferred. lx is 0 or 1, with 1 being preferred. RM9 and RM10 each independently represent a hydrogen atom or an alkyl group, with alkyl groups being more desirable. Here, alkyl groups with 1 to 12 carbon atoms are preferred, with alkyl groups with 1 to 6 carbon atoms being more desirable, and methyl, ethyl, propyl, and butyl groups being more desirable, with methyl being the most desirable. RM11, RM12, RM13, and RM14 each independently represent a hydrogen atom or an organogroup. Alkyl groups are preferred, especially alkyl groups with 1 to 12 carbon atoms, and ideally alkyl groups with 1 to 6 carbon atoms. Methyl, ethyl, propyl, and butyl groups are also preferred, with methyl being the most desirable. RM12 and RM13 are preferably alkyl groups, while RM11 and RM14 are preferably hydrogen atoms. RM15 each independently represents an alkyl group with 1 to 10 carbon atoms, an alkoxy group with 1 to 10 carbon atoms, an alkylthio group with 1 to 10 carbon atoms, a cycloalkyl group with 3 to 10 carbon atoms, an aryl group with 6 to 10 carbon atoms, an aryloxy group with 6 to 10 carbon atoms, an arylthio group with 6 to 10 carbon atoms, a halogen atom, a hydroxyl or mercapto group, preferably an alkyl group with 1 to 4 carbon atoms, a cycloalkyl group with 3 to 6 carbon atoms, or an aryl group with 6 to 10 carbon atoms. px represents an integer from 0 to 3, with 0 to 2 being ideal, 0 or 1 being better, and 0 being even better. nx represents an integer from 1 to 20. nx can also be an integer less than 10. Furthermore, the resin composition of this embodiment may contain only one compound represented by the formula (M1) and at least two different values of nx, or it may contain two or more compounds.When containing two or more compounds, for the compound represented by formula (M1) in the resin composition to have a low melting point (low softening point), low melt viscosity, and excellent workability, the average value of nx (average number of repeating units) n is preferably 0.92 or higher, more preferably 0.95 or higher, more preferably 1.0 or higher, and even more ideally 1.1 or higher. Furthermore, n is preferably 10.0 or lower, more preferably 8.0 or lower, more preferably 7.0 or lower, even more preferably 6.0 or lower, and 5.0 or lower is also acceptable. The same applies to compounds represented by formulas (M1-2) and (M1-3) described later. The compound represented by formula (M1) is preferably a compound represented by the following formula (M1-1). [Chemical 45] In formula (M1-1), RM21, RM22, RM23, and RM24 each independently represent a hydrogen atom or an organic group. RM25 and RM26 each independently represent a hydrogen atom or an alkyl group. RM27, RM28, RM29, and RM30 each independently represent a hydrogen atom or an organic group. RM31 and RM32 each independently represent a hydrogen atom or an alkyl group. RM33, RM34, RM35, and RM36 each independently represent a hydrogen atom or an organic group. RM37, RM38, and RM39 each independently represent a hydrogen atom or an alkyl group. nx represents an integer from 1 to 20.
[0087] In the formula, RM21, RM22, RM23, and RM24 each independently represent a hydrogen atom or an organic group. It is preferred that the organic group is alkyl, more preferably alkyl with 1 to 12 carbon atoms, and ideally alkyl with 1 to 6 carbon atoms. Methyl, ethyl, propyl, and butyl are more ideal, with methyl being particularly preferred. RM21 and RM23 are preferably alkyl, and RM22 and RM24 are preferably hydrogen atoms. RM25 and RM26 each independently represent a hydrogen atom or an alkyl group, with alkyl being preferred. It is preferred that the alkyl group is alkyl with 1 to 12 carbon atoms, more preferably alkyl with 1 to 6 carbon atoms, with methyl, ethyl, propyl, and butyl being more ideal, with methyl being particularly preferred. RM27, RM28, RM29, and RM30 each independently represent a hydrogen atom or an organic group, with hydrogen being preferred. Here, the organogroup is preferably alkyl, more preferably alkyl with 1 to 12 carbons, and even more ideally alkyl with 1 to 6 carbons. Methyl, ethyl, propyl, and butyl are more ideal, with methyl being the most preferred. RM31 and RM32 each independently represent a hydrogen atom or an alkyl group, with alkyl being preferred. Here, the alkyl group is preferably alkyl with 1 to 12 carbons, more preferably alkyl with 1 to 6 carbons. Methyl, ethyl, propyl, and butyl are more ideal, with methyl being the most preferred. RM33, RM34, RM35, and RM36 each independently represent a hydrogen atom or an organogroup. Here, the organogroup is preferably alkyl, more preferably alkyl with 1 to 12 carbons, and even more ideally alkyl with 1 to 6 carbons. Methyl, ethyl, propyl, and butyl are more ideal, with methyl being the most preferred. RM33 and RM36 are preferably hydrogen atoms, while RM34 and RM35 are preferably alkyl. RM37, RM38, and RM39 each independently represent a hydrogen atom or an alkyl group, with alkyl being the most preferred. Here, alkyl groups with 1 to 12 carbon atoms are preferred, alkyl groups with 1 to 6 carbon atoms are even better, and methyl, ethyl, propyl, and butyl are more desirable, with methyl being the most preferred. nx represents an integer from 1 to 20. nx can also be an integer less than 10.
[0088] The compound represented by formula (M1-1) is preferably represented by the compound represented by formula (M1-2). [Chemical 46] In formula (M1-2), RM21, RM22, RM23, and RM24 each independently represent a hydrogen atom or an organic group. RM25 and RM26 each independently represent a hydrogen atom or an alkyl group. RM27, RM28, RM29, and RM30 each independently represent a hydrogen atom or an organic group. RM31 and RM32 each independently represent a hydrogen atom or an alkyl group. RM33, RM34, RM35, and RM36 each independently represent a hydrogen atom or an organic group. RM37, RM38, and RM39 each independently represent a hydrogen atom or an alkyl group. nx represents an integer from 1 to 20.
[0089] In formula (M1-2), R M21, R M22, R M23, R M24, R M25, R M26, R M27, R M28, R M29, R M30, R M31, R M32, R M33, R M34, R M35, R M36, R M37, R M38, R M39, and nx are all synonyms of R M21, R M22, R M23, R M24, R M25, R M26, R M27, R M28, R M29, R M30, R M31, R M32, R M33, R M34, R M35, R M36, R M37, R M38, R M39, and nx in formula (M1-1), and their ideal ranges are also the same.
[0090] The compound represented by formula (M1-1) is preferably represented by the compound represented by formula (M1-3), and even more preferably represented by the compound represented by formula (M1-4). [Chemical Engineering 47] In formula (M1-3), nx represents an integer from 1 to 20. An integer less than 10 is also acceptable. [Chemical Engineering 48] In formula (M1-4), nx represents an integer from 1 to 20. An integer less than 10 is also acceptable.
[0091] It is preferable that the molecular weight of the compound represented by formula (M1) is 500 or higher, more preferably 600 or higher, and even more preferably 700 or higher. By having a molecular weight of 500 or higher than the aforementioned lower limit, the low dielectric properties (Dk and / or Df) and low water absorption of the obtained cured material tend to be further improved. Furthermore, it is preferable that the molecular weight of the compound represented by formula (M1) is 10,000 or lower, more preferably 9,000 or lower, more preferably 7,000 or lower, even more preferably 5,000 or lower, and ideally 4,000 or lower. By having a molecular weight of 4,000 or lower than the aforementioned upper limit, the heat resistance and workability of the obtained cured material tend to be further improved.
[0092] The compound represented by formula (M1) preferably has a maleimide equivalent of 50 g / eq. or more, more preferably 100 g / eq. or more, and even more preferably 200 g / eq. or more. The aforementioned upper limit of the maleimide equivalent is preferably 2000 g / eq. or less, more preferably 1000 g / eq. or less, and even more preferably 800 g / eq. or less. Here, the maleimide equivalent represents the mass of the maleimide compound per 1 maleimide equivalent. When the maleimide equivalent of the compound represented by formula (M1) falls within the above range, the obtained cured product tends to have improved low dielectric properties (Dk and / or Df), low water absorption, heat resistance, and workability.
[0093] For the compound represented by formula (M1), the molecular weight distribution Mw / Mn calculated by gel permeation chromatography (GPC) is preferably 1.0~4.0, more preferably 1.1~3.8, more preferably 1.2~3.6, and even better 1.3~3.4. When the Mw / Mn of the compound represented by formula (M1) falls within the above range, the obtained cured material tends to have improved low dielectric properties (Dk and / or Df), low water absorption, heat resistance, and workability.
[0094] Other details of the compounds represented by formula (M1) can be found in International Publication No. 2020-217679, which is incorporated herein by reference.
[0095] [Chemical 49] In formula (M2), R 54 each independently represents a hydrogen atom or a methyl group, and n 4 represents an integer greater than or equal to 1. It is preferable that n 4 is an integer from 1 to 10, more preferably from 1 to 5, more preferably from 1 to 3, and 1 or 2 is even better, though 1 is also acceptable. The compound represented by formula (M2) may also be a mixture of compounds with different n 4, and a mixture is preferred. Furthermore, as described in the section on compounds represented by formula (M0), a mixture of compounds with different other parts is also acceptable. [Chemical 50] In formula (M3), R 55 each independently represents a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, or a phenyl group, and n 5 represents an integer greater than or equal to 10. It is preferable that R 55 is selected from the group consisting of hydrogen atom, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tributyl, n-pentyl, and phenyl, with hydrogen atom and / or methyl group being more preferred, and hydrogen atom being even more preferred. n 5 is preferably an integer between 1 and 5, more ideally an integer between 1 and 3, and even more ideally 1 or 2. The compound represented by formula (M3) may also be a mixture of compounds with n 5 different parts, and a mixture is preferred. Also, as mentioned in the section on compounds represented by formula (M0), a mixture of compounds with other different parts is also acceptable. [Chemical 51] In formula (M4), R 56 each independently represents a hydrogen atom, a methyl group, or an ethyl group, and R 57 each independently represents a hydrogen atom or a methyl group. It is preferred that R 56 each independently represents a methyl group or an ethyl group, it is even more preferred that R 56 of the two benzene rings each represents a methyl group and an ethyl group, and it is preferred that R 57 represents a methyl group.
[0096] [Chemical 52] In formula (M5), R 58 each independently represents a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, or a phenyl group; R 59 each independently represents a hydrogen atom or a methyl group; and n 6 represents an integer greater than or equal to 1. It is preferable that each of R 58 is selected from the group consisting of hydrogen atoms, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tributyl, n-pentyl, and phenyl, with hydrogen atoms and / or methyl being more preferred, and hydrogen atoms being even more preferred. Methyl is preferred for R 59. It is ideal that n 6 is an integer from 1 to 10, more preferably from 1 to 5, more preferably from 1 to 3, and 1 or 2 is even more preferred, though 1 is also acceptable. The compound represented by formula (M5) may be a mixture of compounds with different n 6, and a mixture is preferred. Furthermore, as described in the section on compounds represented by formula (M0), a mixture of compounds with different other parts may also be acceptable.
[0097] Maleimimine compound (M6) is a compound having the constituent units represented by formula (M6) and maleimimine groups at both ends of the molecular chain. [Chemical 53] In formula (M6), R 61 represents a linear or branched alkyl group having 1 to 16 carbon atoms, or a linear or branched alkenyl group having 2 to 16 carbon atoms. R 62 represents a linear or branched alkyl group having 1 to 16 carbon atoms, or a linear or branched alkenyl group having 2 to 16 carbon atoms. R 63 each independently represents a linear or branched alkyl group having 1 to 16 carbon atoms, or a linear or branched alkenyl group having 2 to 16 carbon atoms. n each independently represents an integer from 0 to 10. Details of the maleimide compound (M6) and its manufacturing method can be found in paragraphs 0061 to 0066 of International Publication No. 2020 / 262577, which is incorporated herein by reference.
[0098] Maleimine compound (M7) is a maleimine compound formed by reacting an aromatic amine compound (a1) having an alkyl group of 1 to 3 or less, an aromatic divinyl compound (a2) having 2 vinyl groups, and maleic anhydride as reactants (1). Maleimine compound (M7) is preferably a compound represented by formula (M7). [Chemical 54] In formula (M7) above, R1 independently represents each of the aforementioned alkyl groups; R2 independently represents each of the following groups: alkyl, alkoxy, or alkylthio group having 1 to 10 carbon atoms; aryl, aryloxy, or arylthio group having 6 to 10 carbon atoms; cycloalkyl group having 3 to 10 carbon atoms; halogen atom; hydroxyl group; or mercapto group; R3, R4, R5, and R6 independently represent each of the following groups: hydrogen atom or methyl group, and one of R3 and R4 is a hydrogen atom and the other is a methyl group; one of R5 and R6 is a hydrogen atom and the other is a methyl group; X1 represents the substituent represented by formula (x); [Chemical 55] In formula (x), R7 and R8 independently represent each of the following groups: hydrogen atom or methyl group, and one of R7 and R8 is a hydrogen atom and the other is a methyl group; R 9 represents alkyl, alkoxy, or alkylthio groups with 1 to 10 carbon atoms; aryl, aryloxy, or arylthio groups with 6 to 10 carbon atoms; cycloalkyl groups with 3 to 10 carbon atoms; halogen atoms; hydroxyl groups; or mercapto groups, where t represents an integer from 0 to 4. r represents the average number of substitutions (X1) of each benzene ring bonded to X1, and is represented as a number from 0 to 4. p represents an integer from 1 to 3, q represents an integer from 0 to 4, and k represents an integer from 1 to 100.
[0099] For details of the polymaleimide compound (M7) used in this embodiment, please refer to the description in Japanese Patent No. 7160151, the contents of which are incorporated herein by reference.
[0100] Maliimines can be manufactured using known methods and can also be commercially available. Commercially available products, for example: compounds represented by formula (M0) include "BMI-80" manufactured by KI Chemical Co., Ltd.; compounds represented by formula (M1) include "NE-X-9470S" manufactured by DIC Co., Ltd.; compounds represented by formula (M2) include "BMI-2300" manufactured by Yamato Chemical Co., Ltd.; compounds represented by formula (M3) include "MIR-3000-70MT" manufactured by Nippon Kayaku Co., Ltd.; compounds represented by formula (M4) include "BMI-70" manufactured by KI Chemical Co., Ltd.; compounds represented by formula (M5) include "MIR-5000" manufactured by Nippon Kayaku Co., Ltd.; maleimide compounds (M6) include "MIZ-001" manufactured by Nippon Kayaku Co., Ltd.; and maleimide compounds (M7) include "NE-X-9500" manufactured by DIC Co., Ltd.
[0101] Furthermore, maleimide compounds other than those mentioned above, such as: oligomers of N-phenylmaleimide, N-cyclohexylmaleimide, phenylmethanemaleimide, m-phenylbismaleimide, 4-methyl-1,3-phenylbismaleimide, 1,6-bismaleimide-(2,2,4-trimethyl)hexane, 4,4'-diphenyl ether bismaleimide, 4,4'-diphenyl bismaleimide, 1,3-bis(3-maleimide phenoxy)benzene, 1,3-bis(4-maleimide phenoxy)benzene, and prepolymers thereof, prepolymers of such maleimides and amines, etc. Among them, monofunctional maleimide compounds such as N-phenylmaleimide and N-cyclohexylmaleimide tend to produce resin compositions that provide excellent curing properties by being used in combination with polymers having structural units represented by the following formula (V).
[0102] When the resin composition of this embodiment contains a maleimide compound, the lower limit of its content is preferably 1 part by mass or more, more preferably 5 parts by mass or more, more preferably 10 parts by mass or more, more preferably 20 parts by mass or more, and more than 25 parts by mass or more, relative to 100 parts by mass of the resin solids in the resin composition. By having a maleimide compound content of 1 part by mass or more, the low dielectric properties and flame retardancy of the obtained cured product tend to be improved. Furthermore, the upper limit of the maleimide compound content is preferably 70 parts by mass or less, more preferably 50 parts by mass or less, and 40 parts by mass or less, relative to 100 parts by mass of the resin solids in the resin composition. By having a maleimide compound content of 70 parts by mass or less, the peel strength and low water absorption of the metal foil tend to be improved. The resin composition of this embodiment may contain only one type of maleimide compound, or it may contain two or more types. When two or more are contained, the total amount within the above-mentioned range is preferred. Furthermore, the resin composition in this embodiment may also be substantially free of maleimide compounds. "Substantially free" means that the content of maleimide compounds relative to 100 parts by weight of the resin solids in the resin composition is less than 1 part by weight, less than 0.1 parts by weight is preferred, and less than 0.01 parts by weight is even more preferred.
[0103] <<Cyanate Ester Compound>> The resin composition of this embodiment may also contain a cyanate ester compound. The cyanate ester compound is not particularly limited as long as it contains 1 or more (preferably 2 to 12, more preferably 2 to 6, even more preferably 2 to 4, more preferably 2 or 3, more preferably 2) cyanate ester groups (cyanoxy groups) within its molecule; it can be widely used in compounds commonly used in the field of printed circuit boards.
[0104] The cyanate ester compound is preferably a cyanate ester compound commonly used in printed circuit boards, having two or more aromatic moieties substituted with at least one cyanooxy group. Specifically, the lower limit of the number of cyanooxy groups in the cyanate ester compound is preferably 2 or more, and more preferably 3 or more. By having values above the above lower limit, the heat resistance tends to be further improved. Furthermore, the upper limit of the number of cyanooxy groups is preferably 100 or less, and more preferably 50 or less. Furthermore, the cyanate ester compound is preferably characterized by excellent low dielectric properties (Dk and / or Df) in its cured form. For example, the dielectric constant (Dk) of the cured cyanate ester compound at a frequency of 10 GHz, measured by the resonant cavity perturbation method, is preferably 4.0 or less, and more preferably 3.5 or less. Furthermore, the aforementioned lower limit of dielectric constant, for example, 2.0 or more, is practical. Furthermore, for the cured product of cyanate compound (B), a dielectric loss tangent (Df) at a frequency of 10 GHz, measured by the resonant cavity perturbation method, is preferably 0.02 or less, and more preferably 0.015 or less. Also, the aforementioned lower limit value of the dielectric loss tangent, for example, 0.0001 or more, is practical. The dielectric constant and dielectric loss tangent can be measured, for example, according to the methods described in the examples (curing conditions, measurement conditions).
[0105] Furthermore, the heat resistance of the cured product of the cyanate ester compound is preferably high. For the cured product of the cyanate ester compound, a glass transition temperature of 150°C or higher, more preferably 180°C or higher, and even more preferably 200°C or higher, as determined by the dynamic viscoelasticity test according to JIS C6481, is preferred. By achieving a glass transition temperature above the aforementioned lower limit, a cured product with excellent heat resistance can be obtained.
[0106] For cyanate ester compounds, a weight-average molecular weight (MAM) of 200 or higher, more preferably 300 or higher, and even more preferably 400 or higher, as measured by GPC, is preferred. A MAM above the aforementioned lower limit tends to improve heat resistance. Furthermore, a MAM of 1000 or lower, more preferably 900 or lower, and even more preferably 800 or lower, is preferred. A MAM below the aforementioned upper limit tends to improve formability and processability.
[0107] The ideal range of cyanate compounds can be referred to paragraphs 0028 to 0033 of International Publication No. 2021 / 172317, the contents of which are incorporated herein by reference.
[0108] An ideal cyanate compound is selected from at least one of the following groups: phenol varnish type cyanate compound, naphthol aralkyl type cyanate compound (naphthol aralkyl type cyanate), naphthyl ether type cyanate compound, biphenyl aralkyl type cyanate compound, xylene resin type cyanate compound, phenol methane type cyanate compound, adamantane skeleton type cyanate compound, bisphenol M type cyanate compound, and bisphenol A type cyanate compound. Among these, considering the viewpoint of further improving low water absorption, it is preferable to select at least one from the group consisting of phenolic varnish-type cyanate compounds, naphthol aralkyl-type cyanate compounds, naphthyl ether-type cyanate compounds, xylene resin-type cyanate compounds, bisphenol M-type cyanate compounds, and bisphenol A-type cyanate compounds; it is even more preferable to select at least one from the group consisting of phenolic varnish-type cyanate compounds, naphthol aralkyl-type cyanate compounds, naphthyl ether-type cyanate compounds, bisphenol A-type cyanate compounds, and bisphenol M-type cyanate compounds; it is even more preferable to select at least one from the group consisting of phenolic varnish-type cyanate compounds, naphthol aralkyl-type cyanate compounds, and bisphenol A-type cyanate compounds; naphthol aralkyl-type cyanate compounds and / or bisphenol A-type cyanate compounds are even more preferable; and naphthol aralkyl-type cyanate compounds are the most ideal.
[0109] Naphthol aralkyl cyanate compounds are more preferably represented by the formula (N1).
[0110] Formula (N1) [Chemical 56] In Formula (N1), R3 independently represents a hydrogen atom or a methyl group, and n3 represents an integer greater than or equal to 1.
[0111] In formula (N1), R3 independently represents either a hydrogen atom or a methyl group, with hydrogen atom being preferred. In formula (N1), n3 is an integer greater than or equal to 1, preferably an integer from 1 to 50, even more preferably an integer from 1 to 20, even more preferably an integer from 1 to 10, and even more ideally an integer from 1 to 6.
[0112] Furthermore, the phenolic varnish-type cyanate compound is not particularly limited, for example, the compound represented by formula (VII) is preferred. [Chemical 57] In formula (VII), R 6 each independently represents a hydrogen atom or a methyl group, and n7 represents an integer greater than 1.
[0113] In formula (VII), R6 independently represents a hydrogen atom or a methyl group, with hydrogen atom being preferred. In formula (VII), n7 is an integer greater than or equal to 1, preferably an integer from 1 to 20, more preferably an integer from 1 to 10, and even more preferably an integer from 1 to 6.
[0114] Bisphenol A type cyanate compounds may also be selected from one or more of the group consisting of prepolymers of 2,2-bis(4-cyanoxyphenyl)propane and 2,2-bis(4-cyanoxyphenyl)propane.
[0115] These cyanate compounds can be prepared using known methods, or commercially available products can be used. Furthermore, cyanate compounds having a naphthol aralkyl skeleton, naphthyl ether skeleton, xylene skeleton, phenyl phenol methane skeleton, or adamantane skeleton have a larger functional group equivalent number and fewer unreacted cyanate groups; therefore, resin compositions using these compounds tend to have better low water absorption. Also, mainly due to having an aromatic skeleton or adamantane skeleton, they tend to have improved plating adhesion.
[0116] When the resin composition of this embodiment contains a cyanate ester compound, the lower limit of its content relative to 100 parts by mass of the resin solids in the resin composition is preferably 1 part by mass or more, more preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and 20 parts by mass or more is also acceptable. By having a cyanate ester compound content of 100 parts by mass or more, the heat resistance, flame retardancy, chemical resistance, low dielectric constant, low dielectric loss tangent, and insulation tend to be improved. The upper limit of the cyanate ester compound content, when the resin composition of this embodiment contains a cyanate ester compound, is preferably 70 parts by mass or less relative to 100 parts by mass of the resin solids in the resin composition, more preferably 60 parts by mass or less, more preferably 50 parts by mass or less, and 40 parts by mass or less, and 30 parts by mass or less is also acceptable. The resin composition of this embodiment may contain only a cyanate ester compound or may contain two or more. When containing two or more, the total amount within the above-mentioned range is preferred. Furthermore, the resin composition in this embodiment may be substantially free of cyanate ester compounds. "Substantially free" means that the content of cyanate ester compounds is less than 1 part by mass, preferably less than 0.1 parts by mass, and more preferably less than 0.01 parts by mass relative to 100 parts by mass of the resin solids in the resin composition.
[0117] <<Epoxy Compound>> The resin composition of this embodiment may also contain an epoxy compound. The epoxy compound is not particularly limited as long as it is a compound or resin having one or more epoxy groups (preferably 2-12, more preferably 2-6, even more preferably 2-4, preferably 2 or 3, even more preferably 2) per molecule, and can be widely used in the field of printed circuit boards. Examples of epoxy compounds include: bisphenol A type epoxy resin, bisphenol E type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, phenolic varnish type epoxy resin, bisphenol A phenolic varnish type epoxy resin, epoxy propylene ester type epoxy resin, aralkylphenolic varnish type epoxy resin, biphenyl aralkyl type epoxy resin, naphthyl ether type epoxy resin, cresol phenolic varnish type epoxy resin, polyfunctional phenol type epoxy resin, and naphthyl type epoxy resin. Anthracene-type epoxy resins, naphthalene-based modified phenolic varnish epoxy resins, phenolic aralkyl-type epoxy resins, naphtholic aralkyl-type epoxy resins, dicyclopentadiene-type epoxy resins, biphenyl-type epoxy resins, alicyclic epoxy resins, polyol-type epoxy resins, phosphorus-containing epoxy resins, glycidyl amine, glycidyl ester, compounds obtained by epoxidation of double bonds in butadiene and other materials, and compounds obtained by reacting hydroxyl-containing polysiloxane resins with epichlorohydrin, etc. Using these improves the moldability and adhesion of the resin composition. Among these, considering the improvement of flame retardancy and heat resistance, biphenyl aralkyl-type epoxy resins, naphthyl ether-type epoxy resins, polyfunctional phenolic epoxy resins, and naphthalene-type epoxy resins are preferred, with biphenyl aralkyl-type epoxy resins being even better.
[0118] In this embodiment, the resin composition preferably contains an epoxy compound within a range that does not impair the effects of the present invention. Considering formability and adhesion, when the resin composition of this embodiment contains an epoxy compound, its content relative to 100 parts by mass of the resin solids in the resin composition is preferably 0.1 parts by mass or more, more preferably 1 part by mass or more, and even more preferably 2 parts by mass or more. With an epoxy compound content of 0.1 parts by mass or more, the peel strength and toughness of the metal foil tend to improve. The upper limit of the epoxy compound content, when the resin composition of this embodiment contains an epoxy compound, relative to 100 parts by mass of the resin solids in the resin composition, is preferably 50 parts by mass or less, more preferably 30 parts by mass or less, more preferably 20 parts by mass or less, even more preferably 10 parts by mass or less, and 8 parts by mass or less, and 5 parts by mass or less are also acceptable. With an epoxy compound content of 50 parts by mass or less, the electrical properties of the obtained cured product tend to improve. The resin composition in this embodiment may contain only one type of epoxy compound, or it may contain two or more types. When it contains two or more types, the total amount within the range described above is preferred. Furthermore, the resin composition in this embodiment may also be substantially free of epoxy compounds. "Substantially free" means that the content of epoxy compounds is less than 0.1 parts by mass relative to 100 parts by mass of the resin solids in the resin composition, preferably less than 0.01 parts by mass, and less than 0.001 parts by mass is also acceptable.
[0119] <<Phenolic Compounds>> The resin composition of this embodiment may also contain phenolic compounds. For details on phenolic resins, please refer to paragraph 0049 of International Publication No. 2021 / 172317, the contents of which are incorporated herein by reference.
[0120] The resin composition of this embodiment preferably contains a phenolic compound within a range that does not impair the effects of the present invention. When the resin composition of this embodiment contains a phenolic compound, its content is preferably 0.1 parts by mass or more, and preferably 50 parts by mass or less, relative to 100 parts by mass of the resin solids in the resin composition. The resin composition of this embodiment may contain only one type of phenolic compound, or it may contain two or more types. When it contains two or more types, the total amount is preferably within the above-mentioned range. Furthermore, the resin composition of this embodiment may also be substantially free of phenolic compounds. Substantially free means that the content of the phenolic compound is less than 0.1 parts by mass relative to 100 parts by mass of the resin solids in the resin composition.
[0121] <<Compounds Containing (Methyl)Allyl Groups>> The resin composition of this embodiment preferably includes compounds containing (methyl)allyl groups, and more preferably includes compounds containing allyl groups. Furthermore, compounds containing (methyl)allyl groups are preferably compounds containing two or more (methyl)allyl groups, and more preferably compounds containing two or more allyl groups. The compound containing (methyl)allyl is preferably composed of at least one selected from the group consisting of (methyl)allyl isocyanurate compounds, tri(methyl)allyl cyanurate compounds, (methyl)allyl-substituted nadicliimide compounds, (methyl)allyl compounds having a glycourea structure, and diallyl phthalate. It is even more preferable that it contains at least one selected from the group consisting of (methyl)allyl isocyanurate compounds, (methyl)allyl-substituted nadicliimide compounds, and (methyl)allyl compounds having a glycourea structure. It is even more preferable that it contains (methyl)allyl isocyanurate compounds and / or (methyl)allyl-substituted nadicliimide compounds. It is even more desirable that it contains (methyl)allyl-substituted nadicliimide compounds.
[0122] Tri(methyl)allyl cyanurate compounds, such as tri(methyl)allyl cyanurate compounds (e.g., cyanurate triallyl cyanurate with the structure disclosed below). [Chemical 58] Furthermore, compounds containing (methyl)allyl groups, such as resins containing allyl groups as described in International Publication No. 2022 / 210095 (e.g., compounds described in Synthesis Examples 3, 4, 6, 20, and 22 of the same publication), are included in this specification.
[0123] When the resin composition of this embodiment contains a compound containing (methyl)allyl, its molecular weight is preferably 195 or higher, more preferably 300 or higher, more preferably 400 or higher, and even more ideally 500 or higher. By being at or above the aforementioned lower limit, there is a tendency to further improve low dielectric properties and heat resistance. The molecular weight of the compound containing (methyl)allyl is preferably 3000 or lower, more preferably 2000 or lower, more preferably 1000 or lower, and even more ideally 800 or lower. By being at or below the aforementioned upper limit, there is a tendency to further improve low thermal expansion.
[0124] When the resin composition of this embodiment contains a compound containing (methyl)allyl, its content relative to 100 parts by mass of the resin solids in the resin composition is preferably 1 part by mass or more, more preferably 3 parts by mass or more, more preferably 5 parts by mass or more, and 10 parts by mass or more is also acceptable. By having the content of the compound containing (methyl)allyl at or above the aforementioned lower limit, there is a tendency for improved moldability and heat resistance. Furthermore, the upper limit of the content of the compound containing (methyl)allyl is preferably 40 parts by mass or less, more preferably 30 parts by mass or less, and even more preferably 20 parts by mass or less, relative to 100 parts by mass of the resin solids in the resin composition. By having the content of the compound containing (methyl)allyl at or below the aforementioned upper limit, there is a tendency for improved low thermal expansion. The resin composition of this embodiment may contain only one compound containing (methyl)allyl, or it may contain two or more. When containing two or more, the total amount within the aforementioned range is preferred.
[0125] <<<(Methyl)allyl isocyanurate compounds>>> (Methyl)allyl isocyanurate compounds are not particularly limited as long as they have two or more (methyl)allyl groups and an isocyanurate ring (urate skeleton). (Methyl)allyl isocyanurate compounds have a large number of (methyl)allyl groups that serve as crosslinking points, thus they tend to harden firmly with resin (A), polyphenylene ether compound (B), and other resin components (e.g., other compounds (C)), and have a tendency to produce cured products with low dielectric properties (Dk and / or Df) and excellent heat resistance. (Methyl)allyl isocyanurate compounds are preferably those represented by formula (TA). Formula (TA) [Chemical 59] In formula (TA), RA represents a substituent.
[0126] In formula (TA), RA represents a substituent, and substituents with a formula weight of 15 to 500 are preferred.
[0127] The first example of RA is an alkyl group having 1 to 22 carbon atoms, or an alkenyl group having 2 to 22 carbon atoms. By using allyl compounds having 1 to 22 carbon atoms or an alkenyl group having 2 to 22 carbon atoms, a resin composition with excellent crosslinking properties and high hardness can be provided. Therefore, even when the resin composition does not contain a substrate such as glass cloth, cracking during etching processes can still be suppressed. From the perspective of improving operability, 3 or more carbon atoms in the aforementioned alkyl and / or alkenyl groups is ideal, 8 or more is better, 12 or more is also acceptable, and 18 or less is also acceptable. Therefore, the resin flowability of the resin composition becomes good, and it is believed that the circuit filling properties are improved when using the resin composition of this embodiment to fabricate multilayer circuit boards, etc.
[0128] The second example of RA is a group containing an allyl isocyanurate group. When RA contains an allyl isocyanurate group, it is preferable that the compound represented by formula (TA) is the compound represented by formula (TA-1). Formula (TA-1) [Chemical 60] In formula (TA-1), RA2 is a divalent linker.
[0129] In formula (TA-1), RA2 is preferably a divalent linker with a formula weight of 54 to 250, more preferably a divalent linker with a formula weight of 54 to 250 and carbon atoms at both ends, and even more preferably an aliphatic hydrocarbon group with 2 to 20 carbon atoms (however, the aliphatic hydrocarbon group may also contain an ether group or a hydroxyl group). More specifically, RA2 is preferably a group represented by any of the following formulas (i) to (iii). [Chemical 61] In formulas (i) to (iii), pc1 represents the number of repeating units of the methylene group, which is an integer from 2 to 18. pc2 represents the number of repeating units of the oxyethyl group, which is 0 or 1. * indicates the bonding site. The aforementioned pc1 is preferably an integer from 2 to 10, more preferably an integer from 3 to 8, and more preferably an integer from 3 to 5. The aforementioned pc2 may be 0 or 1, but is preferably 1.
[0130] The third example of RA is a phosphorus-based substituent.
[0131] RA2 is the best example of the first one.
[0132] In this embodiment, it is preferable that the reactive group (allyl) equivalent of the compound represented by formula (TA) is 1000 g / eq. or less. If the aforementioned equivalent is 1000 g / eq. or less, it is believed that a higher Tg can be obtained more reliably.
[0133] The aforementioned alkyl groups having 1 to 22 carbon atoms include, for example, straight-chain or branched-chain alkyl groups, such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, octyl, nonyl, decyl, dodecyl, tetradecyl, hexadecyl, octadecyl, icosyl, docosyl, etc. Also, the aforementioned alkenyl groups having 2 to 22 carbon atoms include, for example, allyl, decenyl, etc.
[0134] Specific examples of compounds represented by formula (TA) include: triallyl isocyanurate, 5-octyl-1,3-diallyl isocyanurate, 5-dodecyl-1,3-diallyl isocyanurate, 5-tetradecyl-1,3-diallyl isocyanurate, 5-hexadecyl-1,3-diallyl isocyanurate, 5-octadecyl-1,3-diallyl isocyanurate, 5-eicosyl-1,3-diallyl isocyanurate, 5-docenyl-1,3-diallyl isocyanurate, etc. One or more of these compounds can be used in combination, or they can be used in the form of prepolymers.
[0135] There are no particular limitations on the method of manufacturing the compound represented by formula (TA). For example, it can be obtained by reacting diallyl isocyanurate with a haloalkane in an aprotic polar solvent such as N,N'-dimethylformamide in the presence of alkaline substances such as sodium hydroxide, potassium carbonate, and triethylamine at a temperature of about 60°C to 150°C.
[0136] Furthermore, commercially available products may also be used as compounds represented by formula (TA). Commercially available products are not particularly limited, for example: L-DAIC manufactured by Shikoku Chemical Industries, Ltd., and P-DAIC manufactured by Shikoku Chemical Industries, Ltd., which has phosphorus-based substituents. Triallyl isocyanurate, for example: TAIC manufactured by Shin-Mitsubishi Corporation. Compounds represented by formula (TA-1), for example: DD-1 manufactured by Shikoku Chemical Industries, Ltd.
[0137] The molecular weight of the (methyl)allyl isocyanurate compound (preferably a compound represented by formula (TA)) is preferably 200 or more, more preferably 300 or more, more preferably 400 or more, and even more preferably 500 or more. When the aforementioned molecular weight is above the lower limit, the resulting cured product tends to have improved low dielectric properties (Dk and / or Df) and heat resistance. Furthermore, the molecular weight of the (methyl)allyl isocyanurate compound (preferably a compound represented by formula (TA)) is preferably 3000 or less, more preferably 2000 or less, more preferably 1000 or less, and even more preferably 800 or less. When the aforementioned molecular weight is below the upper limit, the resulting cured product tends to have improved low thermal expansion.
[0138] When the resin composition of this embodiment contains a (methyl)allyl isocyanurate compound, its content is preferably 1 part by mass or more, more preferably 3 parts by mass or more, more preferably 5 parts by mass or more, and 10 parts by mass or more, relative to 100 parts by mass of the resin solids in the resin composition. By having the content of the (methyl)allyl isocyanurate compound at or above the aforementioned lower limit, the resin composition tends to have excellent formability, and the heat resistance and low thermal expansion of the obtained cured product are further improved. Furthermore, the upper limit of the content of the (methyl)allyl isocyanurate compound is preferably 40 parts by mass or less, more preferably 30 parts by mass or less, and 20 parts by mass or less, relative to 100 parts by mass of the resin solids in the resin composition. By having the content of the (methyl)allyl isocyanurate compound at or below the aforementioned upper limit, the heat resistance and low dielectric properties (Dk and / or Df) of the obtained cured product are further improved. The resin composition of this embodiment may contain only one (methyl)allyl isocyanurate compound, or it may contain two or more. When it contains two or more compounds, the total amount is preferably within the range described above.
[0139] <<<(Methyl)allyl-substituted nadicimimine compounds>>> (Methyl)allyl-substituted nadicimimine compounds are not particularly limited as long as the molecule has two or more (methyl)allyl-substituted nadicimimine groups. Specific examples include compounds represented by the following formula (AN). Formula (AN) [Chemical 62] In formula (AN), R1 independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms, and R2 represents an alkyl group having 1 to 6 carbon atoms, an alkyl group, an alkyl group, an alkyl group, an alkyl group, an alkyl group, an alkyl group, an alkyl group, an alkyl group, an alkyl group, an alkyl group, an alkyl group, an alkyl group, or an alkyl group represented by formula (AN-2) or (AN-3). Formula (AN-2) [Chemical 63] In formula (AN-2), R3 represents a methylene group, an isopropylidene group, an alkyl group represented by -C(=O)-, an alkyl group, an alkyl group represented by -S-, or an alkyl group represented by -S(=O)2-. In formula (AN-3) [Chemical 64], R 4 independently represents an alkyl group having 1 to 4 carbon atoms or a cycloalkyl group having 5 to 8 carbon atoms.
[0140] Furthermore, commercially available products may also be used as compounds represented by formula (AN). Commercially available products are not particularly limited, for example: compounds represented by formula (AN-4) (BANI-M (Maruzen Petrochemical Co., Ltd.)), compounds represented by formula (AN-5) (BANI-X (Maruzen Petrochemical Co., Ltd.)), etc. One or more of these may be used, or two or more may be used in combination. Formula (AN-4) [Chemical Engineering 65] Formula (AN-5) [Chemical Engineering 66]
[0141] The molecular weight of the (methyl)ally substituted nadicliimide compound (preferably a compound represented by formula (AN)) is preferably 400 or more, more preferably 500 or more, and 550 or more is also acceptable. The molecular weight of the (methyl)ally substituted nadicliimide compound, being at or above the lower limit mentioned above, tends to have improved low dielectric properties, low thermal expansion, and heat resistance. The molecular weight of the (methyl)ally substituted nadicliimide compound (preferably a compound represented by formula (AN)) is preferably 1500 or less, more preferably 1000 or less, more preferably 800 or less, and 700 or less, or 600 or less is also acceptable. The molecular weight of the (methyl)ally substituted nadicliimide compound, being at or below the upper limit mentioned above, tends to have improved formability and peel strength.
[0142] When the resin composition of this embodiment contains a (methyl)ally substituted nadicliimide compound (preferably a compound represented by formula (AN)), its content relative to 100 parts by mass of the resin solids in the resin composition is preferably 1 part by mass or more, more preferably 3 parts by mass or more, more preferably 5 parts by mass or more, and 10 parts by mass or more is also acceptable. By having the content of the (methyl)ally substituted nadicliimide compound at or above the aforementioned lower limit, there is a tendency for improved formability, low dielectric properties, low thermal expansion, and enhanced heat resistance. Furthermore, the upper limit of the content of the (methyl)ally substituted nadicliimide compound (preferably a compound represented by formula (AN)) relative to 100 parts by mass of the resin solids in the resin composition is preferably 40 parts by mass or less, more preferably 30 parts by mass or less, more preferably 25 parts by mass or less, and 20 parts by mass or less is also acceptable. By keeping the content of (methyl)allyl-substituted nadicimimine compounds below the aforementioned upper limit, there is a tendency for improved formability and peel strength. The resin composition of this embodiment may contain only one type of (methyl)allyl-substituted nadicimimine compound, or it may contain two or more. When containing two or more, the total amount falling within the aforementioned range is preferable.
[0143] <<<(Methyl)allyl compounds having a glycourea structure>>> A (methyl)allyl compound having a glycourea structure is any compound containing two or more glycourea structures and (methyl)allyl groups, without particular limitation. When a (methyl)allyl compound having a glycourea structure is incorporated into a resin composition, the number of (methyl)allyl groups increases, that is, the number of crosslinking points increases. Therefore, similar to (methyl)allyl isocyanurate compounds, it tends to cure firmly with resin (A), polyphenylene ether compound (B), and other resin components (e.g., other compounds (C)) and obtain cured products with low dielectric properties (Dk and / or Df) and excellent heat resistance. In this embodiment, a (methyl)allyl compound having a glycourea structure is preferably a compound represented by formula (GU). In formula (GU) [Chemical 67], each R is independently a hydrogen atom or a substituent, and at least two of R are groups containing (methyl)allyl. In formula (GU), each R is preferably a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or an alkenyl group having 2 to 5 carbon atoms, with an alkenyl group having 2 to 5 carbon atoms being more preferred, (methyl)allyl being more preferred, and allyl being even more preferred. In formula (GU), it is preferable that three or four R are groups containing (methyl)allyl, and even more preferable that four R are groups containing (methyl)allyl.
[0144] Specific examples of compounds represented by formula (GU) include 1,3,4,6-tetraallylglycourea (in formula (GU), R represents allyl compounds).
[0145] Furthermore, commercially available products may also be used for compounds represented by formula (GU). Commercially available products are not particularly limited, for example: TA-G manufactured by Shikoku Chemical Industry Co., Ltd.
[0146] The molecular weight of the (methyl)allyl compound having a glycourea structure (preferably a compound represented by formula (GU)) is preferably 195 or more, more preferably 220 or more, more preferably 250 or more, and 300 or more, or 400 or more is also acceptable. When the molecular weight of the (methyl)allyl compound having a glycourea structure is at or above the lower limit mentioned above, the heat resistance and low thermal expansion of the obtained cured material tend to be further improved. The molecular weight of the (methyl)allyl compound having a glycourea structure (preferably a compound represented by formula (GU)) is preferably 1500 or less, more preferably 1000 or less, more preferably 800 or less, and 700 or less, or 600 or less is also acceptable. When the molecular weight of the (methyl)allyl compound having a glycourea structure is below the upper limit mentioned above, the low dielectric properties (Dk and / or Df) and heat resistance of the obtained cured material tend to be further improved.
[0147] When the resin composition of this embodiment contains a (methyl)allyl compound having a glycourea structure (preferably a compound represented by formula (GU)), its content relative to 100 parts by mass of the resin solids in the resin composition is preferably 1 part by mass or more, more preferably 3 parts by mass or more, more preferably 5 parts by mass or more, and 10 parts by mass or more is also acceptable. By having the content of the (methyl)allyl compound having a glycourea structure at or above the above-mentioned lower limit, the resin composition exhibits excellent formability and tends to further improve the heat resistance and low thermal expansion of the obtained cured product. Furthermore, the upper limit of the content of the (methyl)allyl compound having a glycourea structure (preferably a compound represented by formula (GU)) relative to 100 parts by mass of the resin solids in the resin composition is preferably 40 parts by mass or less, more preferably 30 parts by mass or less, more preferably 25 parts by mass or less, and 20 parts by mass or less is also acceptable. By keeping the content of (methyl)allyl compounds with a glycidyl structure below the aforementioned upper limit, the low dielectric properties (Dk and / or Df) of the obtained cured product tend to be further improved. The resin composition of this embodiment may contain only one type of (methyl)allyl compound with a glycidyl structure, or it may contain two or more types. When containing two or more types, the total amount falling within the aforementioned range is preferred.
[0148] <<Oxycyclobutane Resin>> The resin composition of this embodiment may also contain oxycyclobutane resin. Oxycyclobutane resin is not particularly limited as long as it is a compound having one or more glycidyl groups (preferably 2 to 12, more preferably 2 to 6, more preferably 2 to 4, more preferably 2 or 3, more preferably 2), and can be widely used in the field of printed circuit boards. Oxycyclic butane resins, such as: oxycyclic butane, alkyloxycyclic butanes (e.g., 2-methyloxycyclic butane, 2,2-dimethyloxycyclic butane, 3-methyloxycyclic butane, 3,3-dimethyloxycyclic butane, etc.), 3-methyl-3-methoxymethyloxycyclic butane, 3,3-di(trifluoromethyl)oxycyclic butane, 2-chloromethyloxycyclic butane, 3,3-bis(chloromethyl)oxycyclic butane, biphenyl-type oxycyclic butane, OXT-101 (manufactured by Dong-A Synthetic Co., Ltd.), OXT-121 (manufactured by Dong-A Synthetic Co., Ltd.), etc.
[0149] In the resin composition of this embodiment, it is preferable to contain oxetane resin within a range that does not impair the effects of the present invention. When the resin composition of this embodiment contains oxetane resin, its content is preferably 0.1 parts by mass or more, more preferably 1 part by mass or more, and more preferably 2 parts by mass or more, relative to 100 parts by mass of the resin solids in the resin composition. By having an oxetane resin content of 0.1 parts by mass or more, there is a tendency to improve the peel strength and toughness of the obtained cured metal foil. Regarding the upper limit of the oxetane resin content, when the resin composition of this embodiment contains oxetane resin, it is preferable to have 50 parts by mass or less, more preferably 30 parts by mass or less, more preferably 20 parts by mass or less, more preferably 10 parts by mass or less, and more preferably 8 parts by mass or less, relative to 100 parts by mass of the resin solids in the resin composition. By having an oxetane resin content of 50 parts by mass or less, there is a tendency to improve the electrical properties of the obtained cured material. The resin composition in this embodiment may contain only one type of oxetane resin, or it may contain two or more types. When it contains two or more types, the total amount within the above-mentioned range is preferred. Furthermore, the resin composition in this embodiment may also be substantially free of oxetane resin. "Substantially free" means that the content of oxetane resin is less than 0.1 parts by mass relative to 100 parts by mass of the resin solids in the resin composition.
[0150] <<Benzoan Compound>> The resin composition of this embodiment may also contain benzoan compound. The benzoan compound is not particularly limited as long as it is a compound having two or more (preferably 2 to 12, more preferably 2 to 6, more preferably 2 to 4, more preferably 2 or 3, more preferably 2) dihydrobenzoan rings per molecule, and compounds commonly used in the field of printed circuit boards can be widely used. Benzo[a] compounds, such as: bisphenol A type benzo[a] BA-BXZ (manufactured by Konishi Chemical Co., Ltd.), bisphenol F type benzo[a] BF-BXZ (manufactured by Konishi Chemical Co., Ltd.), bisphenol S type benzo[a] BS-BXZ (manufactured by Konishi Chemical Co., Ltd.), etc.
[0151] It is preferable that the resin composition of this embodiment contains benzo[a] ... "Substantially absent" means that the content of benzo[a] compounds is less than 0.1 parts by weight per 100 parts by weight of the resin solids in the resin composition.
[0152] 〈〈Arylcyclobutene resin〉〉 The resin composition of this embodiment may also contain arylcyclobutene resin. For details, examples of arylcyclobutene resins described in paragraph 0042 of Japanese Patent Application Publication No. 2019-194312 are included in this specification.
[0153] <<Polyamide Resin>> The resin composition of this embodiment may also contain polyamide resin, or it may contain thermosetting polyamide resin. For details, please refer to paragraph 0065 of Japanese Patent Application Publication No. 2019-194312 and paragraph 0063 of Japanese Patent Application Publication No. 6951829, the contents of which are incorporated herein by reference.
[0154] <<Polyimide Resin>> The resin composition of this embodiment may also contain polyimide resin, or thermosetting polyimide resin. For details, please refer to paragraphs 0063-0064 of Japanese Patent No. 6951829, which describes polyimide, etc., and the content is incorporated herein by reference.
[0155] <<Perfluoroethylene ether resin>> The resin composition of this embodiment may also contain perfluoroethylene ether resin or perfluorovinyl benzyl ether resin. For details, examples of perfluoroethylene ether resins, etc., described in paragraph 0043 of Japanese Patent Application Publication No. 2019-194312 are included in this specification.
[0156] <<Compounds with styrene groups other than polyphenylene ether compounds (B) with carbon-carbon unsaturated double bonds at the ends>> The resin composition of this embodiment may also contain compounds with styrene groups other than polyphenylene ether compounds (B) with carbon-carbon unsaturated double bonds at the ends. Details of such compounds are illustrated in International Publication No. 2022 / 210095 (e.g., the compounds described in Synthesis Examples 12-16 of the same publication), paragraphs 0029-0038 of Japanese Patent Application Publication No. 2022-85610, and paragraph 0041 of Japanese Patent Application Publication No. 2019-194312, etc., and these contents are incorporated herein by reference.
[0157] <<Compounds with isopropenyl groups other than resins (A) having a dihydroindene skeleton>> The resin composition of this embodiment may also contain compounds with isopropenyl groups other than resins (A) having a dihydroindene skeleton. Details of such compounds are illustrated in International Publication No. 2022 / 210095, which describes resins with isopropenyl groups (e.g., compounds described in Synthesis Examples 1, 2, 7, and 8 of the same publication), and their contents are incorporated herein by reference.
[0158] <<Polyfunctional (meth)acrylate compounds other than the aforementioned polyphenylene ether compound (B) with terminal carbon-carbon unsaturated double bonds>> The resin composition of this embodiment may also contain polyfunctional (meth)acrylate compounds other than the aforementioned polyphenylene ether compound (B) with terminal carbon-carbon unsaturated double bonds. Here, a polyfunctional (meth)acrylate compound refers to a compound containing two or more (meth)acrylic oxy groups per molecule, preferably containing three or more (meth)acrylic oxy groups per molecule. It is preferable that the polyfunctional (meth)acrylate compound has three to five (meth)acrylic oxy groups, more preferably three or four (meth)acrylic oxy groups, and even more preferably three (meth)acrylic oxy groups. It is preferable that the (meth)acrylate compound has a methacrylic oxy group. Polyfunctional (meth)acrylate compounds, due to the large number of (meth)acrylate groups that serve as crosslinking points, can firmly cure with resin (A), polyphenylene ether compound (B), and other resin components (e.g., other compounds (C)), resulting in cured products with low dielectric properties (Dk and / or Df) and excellent heat resistance. Polyfunctional (meth)acrylate compounds are preferably those represented by formula (MA). Formula (MA) [Chemical 68] In formula (MA), R1 represents a hydrogen atom or a substituent, and R2 independently represents a hydrogen atom or a methyl group.
[0159] In formula (MA), R1 represents a hydrogen atom or a substituent, with substituents of formula weight 15 to 500 being more preferred, substituents of formula weight 15 to 300 being more preferred, substituents of formula weight 15 to 100 being more preferred, and substituents of formula weight 15 to 50 being even more ideal.
[0160] R1 is preferably a hydrocarbon group or (meth)acryloxy group, more preferably a hydrocarbon group with 22 or fewer carbon atoms, and even more preferably an alkyl group with 1 to 22 carbon atoms or an alkenyl group with 2 to 22 carbon atoms. By using a compound having an alkyl group with 1 to 22 carbon atoms or an alkenyl group with 2 to 22 carbon atoms, a resin composition with excellent crosslinking properties and high hardness can be provided. Therefore, even when the resin composition does not contain a substrate such as glass cloth, cracking during etching processes can be suppressed. Regarding the aforementioned alkyl and / or alkenyl groups, considering the improvement of operability, 2 or more carbon atoms is ideal, 8 or more is also acceptable, 12 or more is also acceptable, and 18 or less is also acceptable. Therefore, the resin flowability of the resin composition becomes good, and it is believed that the circuit filling properties when using the resin composition of this embodiment to fabricate multilayer circuit boards, etc., will be better.
[0161] In this embodiment, it is preferable that the (meth)acrylate equivalent of the compound represented by formula (MA) is 1000 g / eq. or less. If the aforementioned equivalent is 1000 g / eq. or less, there is a tendency to obtain a higher Tg more reliably. For example, the lower limit of the (meth)acrylate equivalent is 99 g / eq. or more.
[0162] The aforementioned alkyl groups having 1 to 22 carbon atoms are preferably straight-chain alkyl groups having 1 to 22 carbon atoms or branched alkyl groups having 3 to 22 carbon atoms, such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, octyl, nonyl, decyl, dodecyl, tetradecyl, hexadecyl, octadecyl, icosyl, docosyl, etc. Furthermore, the aforementioned alkenyl groups having 2 to 22 carbon atoms are preferably alkenyl groups having 2 to 15 carbon atoms, such as allyl, decenyl, etc.
[0163] Specific examples of compounds represented by formula (MA) include: trimethylolpropane trimethacrylate, trimethylolpropane triacrylate, neopentyl tert-tetra(meth)acrylate, etc. One of them may be used or a combination of two or more, and they may also be used in the form of prepolymers.
[0164] Furthermore, the compound represented by formula (MA) may be a commercially available product. Commercially available products are not particularly limited, for example: trimethylolpropane trimethacrylate, such as "NK ESTER TMPT" manufactured by Shin-Nakamura Chemical Industry (Co., Ltd.).
[0165] It is preferable that the molecular weight of the polyfunctional (meth)acrylate compound is 300 or higher, more preferably 330 or higher, and also acceptable for 400 or higher, and 500 or higher. When the aforementioned molecular weight is above the lower limit, the cured product tends to have improved low dielectric properties (Dk and / or Df) and heat resistance. Furthermore, it is preferable that the molecular weight of the (meth)acrylate compound (preferably a compound represented by formula (MA)) is 3000 or lower, more preferably 2000 or lower, more preferably 1000 or lower, and ideally 800 or lower. When the aforementioned molecular weight is below the upper limit, the cured product tends to have improved low thermal expansion.
[0166] Details of such resins can be found in International Publication No. 2022 / 210095, which describes resins containing (meth)acrylic acid groups (e.g., compounds described in Synthesis Examples 5 and 21 of the same publication) and Japanese Patent No. 6962507, which describes resins containing (meth)acrylic acid groups (e.g., compounds described in Examples 1 to 9), the contents of which are incorporated herein by reference.
[0167] When the resin composition of this embodiment contains a polyfunctional (meth)acrylate compound, its content relative to 100 parts by mass of the resin solids in the resin composition is preferably 1 part by mass or more, more preferably 3 parts by mass or more, more preferably 5 parts by mass or more, and 10 parts by mass or more is also acceptable. When the content of the polyfunctional (meth)acrylate compound is at or above the aforementioned lower limit, the resin composition exhibits excellent formability, and the heat resistance and low thermal expansion properties of the obtained cured product tend to be further improved. Furthermore, when the content of the (meth)acrylate compound is at or below the aforementioned upper limit, it is preferably 40 parts by mass or less, more preferably 30 parts by mass or less, and 20 parts by mass or less is also acceptable. When the content of the polyfunctional (meth)acrylate compound is below the aforementioned upper limit, the heat resistance and low dielectric properties (Dk and / or Df) of the obtained cured product tend to be further improved. The resin composition of this embodiment may contain only one polyfunctional (meth)acrylate compound, or it may contain two or more. When it contains two or more compounds, the total amount is preferably within the range described above.
[0168] <<Elastomer>> The resin composition of this embodiment may also contain an elastomer. The elastomer may be thermoplastic, thermosetting, or neither thermoplastic nor thermosetting, but thermoplasticity is preferred. The elastomer in this embodiment is not particularly limited, and may be selected from at least one of the group consisting of polyisoprene, polybutadiene, styrene-butadiene, butyl rubber, ethylene-propylene rubber, styrene-butadiene-ethylene, styrene-butadiene-styrene, styrene-isoprene-styrene, styrene-ethylene-butene-styrene, styrene-propylene-styrene, fluororubber, polysiloxane rubber, their hydrides, their alkyl compounds, and their copolymers. Furthermore, the elastomer may also include oligomers or polymers with curable vinyl functional groups as described in paragraphs 0044 and 0045 of Japanese Patent Application Publication No. 2019-194312, and polybutadiene resins, which are incorporated herein by reference.
[0169] The number average molecular weight of the elastomer (preferably a thermoplastic elastomer) used in this embodiment is preferably 1000 or more. With a number average molecular weight of 1000 or more, the resulting cured product tends to have better low dielectric properties (Dk and / or Df, especially low dielectric loss tangent). A number average molecular weight of 1500 or more is preferred, 2000 or more is even more preferred, and depending on the application, 600,000 or more, 700,000 or more, and 800,000 or more are also acceptable. The upper limit of the number average molecular weight of the elastomer is preferably 400,000 or less, 350,000 or less is even more preferred, and 300,000 or less is still more preferred. With values below the aforementioned upper limit, the solubility of the elastomer component in the resin composition tends to be improved. When the resin composition of this embodiment contains two or more elastomers, the number average molecular weight of their mixture should preferably conform to the above range.
[0170] The elastomer used in this embodiment is, for example, a resin containing a polybutadiene structure. Part or all of the polybutadiene structure may also be hydrogenated. Specific examples include: B-1000, B-2000, B-3000, BI-2000, BI-3000 manufactured by Nippon Soda Co., Ltd.; and Ricon100, Ricon130, Ricon131, Ricon142, Ricon150, Ricon181, Ricon184 manufactured by Cray Valley Co., Ltd.
[0171] The elastomer used in this embodiment is, for example, a resin having a poly(meth)acrylate structure. Specific examples include TEISANRESIN manufactured by Nagasechemtex, ME-2000, W-197C, KG-15, and KG-3000 manufactured by Negami Kogyo Co., Ltd.
[0172] The elastomer used in this embodiment may include resins containing a polycarbonate structure. Resins containing a polycarbonate structure are sometimes called "polycarbonate resins." Such resins include, for example, carbonate resins without reactive groups, carbonate resins containing hydroxyl groups, carbonate resins containing phenolic hydroxyl groups, carbonate resins containing carboxyl groups, carbonate resins containing acid anhydride groups, carbonate resins containing isocyanate groups, carbonate resins containing carbamate groups, and carbonate resins containing epoxy groups. Here, a reactive group refers to a functional group that can react with other components such as hydroxyl, phenolic hydroxyl, carboxyl, acid anhydride, isocyanate, carbamate, and epoxy groups. Specific examples of polycarbonate resins include FPC0220 and FPC2136 manufactured by Mitsubishi Gas Chemical Co., Ltd., and T6002 and T6001 (polycarbonate diol) manufactured by Asahi Kasei Chemical Co., Ltd.
[0173] The elastomer used in this embodiment is, for example, a resin containing a polysiloxane structure. Specific examples include SMP-2006, SMP-2003PGMEA, SMP-5005PGMEA, KR-510, and SMP-7014-3S manufactured by Shin-Etsu Silicon Power Co., Ltd.
[0174] The elastomer used in this embodiment is, for example, a resin containing a polyalkylene structure and / or a polyalkyloxy group. A polyalkyloxy group with 2 to 15 carbon atoms is preferred, a polyalkyloxy group with 3 to 10 carbon atoms is better, and a polyalkyloxy group with 5 to 6 carbon atoms is especially preferred. Specific examples of resins containing a polyalkylene structure and / or a polyalkyloxy group include PTXG-1000 and PTXG-1800 manufactured by Asahi Kasei Corporation.
[0175] The elastomer used in this embodiment is, for example, a resin containing a polyisoprene structure. Specific examples include KL-610 and KL613 manufactured by Kuraray Co., Ltd.
[0176] The elastomer used in this embodiment is, for example, a resin containing a polyisobutylene structure. Specific examples include SIBSTAR-073T (styrene-isobutylene-styrene triblock copolymer) and SIBSTAR-042D (styrene-isobutylene diblock copolymer) manufactured by Kaneka Corporation.
[0177] In this embodiment, it is preferable that the elastomer contains styrene monomer units and conjugated diene monomer units (hereinafter referred to as "elastomer (e)"). By using such an elastomer (e), the hardened material obtained has better low dielectric properties (Dk and / or Df, especially low dielectric loss tangent).
[0178] The elastomer (e) described above contains styrene monomer units. By containing styrene monomer units, the solubility of the elastomer (e) in resin compositions is improved. Among styrene monomers, such as styrene, α-methylstyrene, p-methylstyrene, divinylbenzene (vinylstyrene), N,N-dimethyl-p-aminoethylstyrene, and N,N-diethyl-p-aminoethylstyrene, styrene, α-methylstyrene, and p-methylstyrene are preferred from the viewpoint of availability and manufacturability. Styrene is particularly preferred. In the elastomer (e) described above, the content of styrene monomer units is ideally in the range of 10-50% by mass of all monomer units, more preferably in the range of 13-45% by mass, and even more preferably in the range of 15-40% by mass. If the content of styrene monomer units is 50% by mass or less, the adhesion and bonding with the substrate are better. Furthermore, if the content is 10% by mass or higher, it tends to suppress the increase in adhesive strength, is less prone to residue and stop marks, and exhibits good peelability between the adhesive surfaces, thus being more ideal. The elastomer (e) may contain only one type of styrene monomer unit or two or more types. When containing two or more types, the above-mentioned range is preferable. The method for determining the content of styrene monomer units in the elastomer (e) of this embodiment can be referred to International Publication No. 2017 / 126469, the contents of which are incorporated herein by reference. The same applies to the conjugated diene monomer units, etc., described later.
[0179] The elastomer (e) described above contains a conjugated diene monomer unit. By containing a conjugated diene monomer unit, the solubility of the elastomer (e) in the resin composition is improved. The conjugated diene monomer is any diene having one pair of conjugated double bonds, without particular limitation. Examples of conjugated diene monomers include: 1,3-butadiene, 2-methyl-1,3-butadiene (isoprene), 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 2-methyl-1,3-pentadiene, 1,3-hexadiene, and farnesene. 1,3-butadiene and isoprene are preferred, with 1,3-butadiene being more ideal. The elastomer (e) may contain only one type of conjugated diene monomer unit, or it may contain two or more types.
[0180] In the above elastomer (e), the mass ratio of styrene monomer units to conjugated diene monomer units is preferably in the range of 5 / 95 to 80 / 20, more preferably in the range of 7 / 93 to 77 / 23, and even more preferably in the range of 10 / 90 to 70 / 30. If the mass ratio of styrene polymer units to conjugated diene monomer units is in the range of 5 / 95 to 80 / 20, the increase in adhesive strength can be suppressed, the adhesive force can be maintained at a high level, and the ease of peeling between the adhesive surfaces becomes good.
[0181] The above elastomer (e) may have its conjugated diene bonds fully hydrogenated, partially hydrogenated, or not hydrogenated.
[0182] The elastomer (e) described above may contain styrene monomer units and conjugated diene monomer units, or it may not contain other monomer units. Other monomer units include, for example, aromatic vinyl compound units other than styrene monomer units. In the elastomer (e) described above, the total amount of styrene monomer units and conjugated diene monomer units is preferably 90% by mass or more, more preferably 95% by mass or more, more preferably 97% by mass or more, and even more ideally 99% by mass or more. As mentioned above, the elastomer (e) may contain only one type of styrene monomer unit and one type of conjugated diene monomer unit, or it may contain two or more types. When it contains two or more types, the total amount is preferably within the above range.
[0183] The elastomer (e) used in this embodiment can be a block polymer or a random polymer. Furthermore, the conjugated diene monomer unit can be a hydrogenated elastomer, an unhydrogenated elastomer, or a partially hydrogenated elastomer; unhydrogenated or partially hydrogenated elastomers are preferred. In one embodiment of this embodiment, the elastomer (e) is a hydrogenated elastomer. Here, a hydrogenated elastomer refers, for example, to one where the double bond of the conjugated diene monomer unit in the elastomer has been hydrogenated, meaning a hydrogenation rate of 100%, but also including those with a hydrogenation rate of 80% or higher. For hydrogenated elastomers, a hydrogenation rate of 85% or higher is ideal, 90% or higher is more preferred, and 95% or higher is even more preferred. In this embodiment, the hydrogenation rate is calculated from the measurement results of 1H-NMR spectroscopy. In one embodiment of this embodiment, the elastomer (e) is an unhydrogenated elastomer. Here, unhydrogenated elastomers refer to those in which the proportion of hydrogenated components in the double bonds of the conjugated diene monomer units within the elastomer, i.e., the hydrogenation rate, is 20% or less. A hydrogenation rate of 15% or less is ideal, 10% or less is better, and 5% or less is even better. On the other hand, partially hydrogenated elastomers refer to those in which only a portion of the double bonds of the conjugated diene monomer units within the elastomer are hydrogenated, typically referring to those with a hydrogenation rate between 20% and 80%.
[0184] Commercially available elastomers (e) used in this embodiment include, for example, SEPTON (registered trademark) 2104, V9461, S8104 manufactured by Kuraray Co., Ltd.; SOE (registered trademark) S1606, S1613, S1609, S1605 manufactured by Asahi Kasei Co., Ltd.; H1041, H1043, P2000, MP10 manufactured by Asahi Kasei Co., Ltd.; and DYNARON (registered trademark) 9901P, TR2250 manufactured by JSR Co., Ltd.
[0185] The elastomer used in this embodiment may also be a liquid diene. Liquid diene refers to a liquid elastomer containing conjugated diene monomer units. Examples of conjugated diene monomers include 1,3-butadiene, 2-methyl-1,3-butadiene (isoprene), 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 2-methyl-1,3-pentadiene, 1,3-hexadiene, and chlorophenene. 1,3-butadiene and isoprene are preferred, with 1,3-butadiene being even more ideal. The liquid diene used in this embodiment includes, for example, liquid polybutadiene, liquid polyisoprene, modified liquid polybutadiene, modified liquid polyisoprene, acrylonitrile-butadiene copolymer, and liquid styrene-butadiene copolymer. Furthermore, regarding the number average molecular weight of liquid dienes, it is acceptable as long as they are liquid at 20°C, without particular limitation, but preferably between 500 and 10,000.
[0186] When the resin composition of this embodiment contains an elastomer (preferably elastomer (e)), its content is preferably 1 part by mass or more, more preferably 5 parts by mass or more, and more preferably 8 parts by mass or more, relative to 100 parts by mass of the resin solids in the resin composition. Depending on the application, it may also be 10 parts by mass or more, or 12 parts by mass or more. By reaching the aforementioned lower limit or above, the dielectric properties (low dielectric loss tangent) tend to be further improved. Furthermore, the upper limit of the elastomer content is preferably 45 parts by mass or less, more preferably 40 parts by mass or less, more preferably 35 parts by mass or less, more preferably 32 parts by mass or less, and ideally 28 parts by mass or less, relative to 100 parts by mass of the resin solids in the resin composition. By reaching the aforementioned upper limit or below, the heat resistance tends to be further improved. The resin composition of this embodiment may contain only one type of elastomer or may contain two or more types. When containing two or more types, the total amount within the above range is preferred. Furthermore, the resin composition in this embodiment may also be substantially free of elastomer. "Substantially free of" means that the content of elastomer is less than 1 part by mass, less than 0.1 parts by mass, and more preferably less than 0.01 parts by mass relative to 100 parts by mass of the resin solids in the resin composition.
[0187] <<Petroleum Resin>> The resin composition of this embodiment may also contain petroleum resin. By containing petroleum resin, the melt viscosity can be reduced. Petroleum resin is a resin obtained by polymerizing the residue after thermal decomposition of petroleum and collection of necessary fractions without isolating unsaturated hydrocarbons, or in the presence or absence of a catalyst. The aforementioned residual fractions are mainly fractions containing C5 fractions (isoprene, isoprene, cyclopentadiene, pentenes, pentanes, etc.) or C9 fractions (vinyltoluene, indene, dicyclopentadiene, etc.).
[0188] Acidic catalysts are preferred for use in the manufacture of petroleum resins. Specifically, boron trifluoride phenol complexes, boron trifluoride ether complexes, aluminum chloride, aluminum bromide, ferric chloride (III), ferric bromide (III), Lewis acids such as zeolite, silicon dioxide, montmorillonite, alumina, fluorinated resins containing sulfonic acid groups, ion exchange resins such as polystyrene resins containing sulfonic acid groups, sulfuric acid, hydrochloric acid, acetic acid, phosphoric acid, oxalic acid, nitric acid, p-toluenesulfonic acid, trifluoroacetic acid, etc. are suitable. Among these, Lewis acids and solid acids that are less likely to cause side reactions and have a fast reaction rate are preferred. Considering ease of acquisition and high reactivity, various boron trifluoride complexes and aluminum chloride are more ideal.
[0189] There is no particular limitation on the weight average molecular weight of petroleum resin, but it is preferably 500 to 10,000, and more preferably 500 to 5,000. By being below the aforementioned upper limit, it is easier to be compatible with other resins, and its solubility in solvents tends to be improved. By being above the aforementioned lower limit, the heat resistance and mechanical strength of the obtained cured product tend to be further improved.
[0190] There are no particular limitations on the softening point of petroleum resin, but a higher softening point is preferred, above 80°C is preferred, and above 100°C is even better. By achieving a value above the aforementioned lower limit, the heat resistance of the hardened material tends to be improved.
[0191] Petroleum resins, such as aliphatic petroleum resins, aromatic petroleum resins, copolymer petroleum resins, and dicyclopentadiene petroleum resins, preferably dicyclopentadiene petroleum resins. Dicyclopentadiene petroleum resins include, for example, resins obtained by polymerizing dicyclopentadiene fractions such as dicyclopentadiene, isopropenylnorcamphene, dimethyldicyclopentadiene, and tricyclopentadiene, and resins obtained by polymerizing dicyclopentadiene fractions with other monomers having unsaturated bonds, preferably unsaturated cyclic olefins.
[0192] The aforementioned unsaturated cyclic olefins, such as cyclopentadiene; 2-norcamphene, 5-methyl-2-norcamphene, 5-ethylidene-2-norcamphene, 5-phenylnorcamphene, 5-propenyl-2-norcamphene, 5-ethylidene-2-norcamphene and other nocamphene monomers; nocamphene monomers with tricyclic or higher forms, such as diethyldicyclopentadiene, dihydrodicyclopentadiene and other tricyclic fractions, tetracyclic and tetracyclic dodecene and other tetracyclic fractions, pentacyclic and pentacyclic and heptacyclic and tetracyclic fractions, and alkyl-substituted, alkylene-substituted, aryl-substituted, etc. of such polycyclic fractions. The aforementioned alkyl-substituted polycyclic compounds include, for example, methyl, ethyl, propyl, and butyl-substituted polycyclic compounds; the aforementioned alkylene-substituted polycyclic compounds include, for example, ethylene-substituted polycyclic compounds; and the aforementioned aryl-substituted polycyclic compounds include, for example, phenyl, tolyl, and naphthyl-substituted polycyclic compounds.
[0193] Furthermore, monomers other than unsaturated cyclic olefins that have unsaturated bonds can also copolymerize olefins with 3 to 12 carbon atoms, such as: propylene, but-1-ene, pent-1-ene, 1,3-pentadiene, hex-1-ene, hepten-1, oct-1-ene, diisobutylene, non-1-ene, dec-1-ene, 4-phenylbut-1-ene, 6-phenylhex-1-ene, 3-methylbut-1-ene, 4-methyl α-olefins such as pent-1-ene, 3-methylpent-1-ene, 3-methylhex-1-ene, 4-methylhex-1-ene, 5-methylhex-1-ene, 3,3-dimethylpent-1-ene, 3,4-dimethylpent-1-ene, 4,4-dimethylpent-1-ene, vinylcyclohexane, and vinylcyclohexene; halogenated α-olefins such as hexafluoropropylene, 2-fluoropropylene, 3-fluoropropylene, and 3,4-dichlorobutene-1.
[0194] Other monomers with unsaturated bonds besides those mentioned above, such as: ethylene, tetrafluoroethylene, fluoroethylene, 1,1-difluoroethylene, trifluoroethylene; styrene, p-methylstyrene, o-methylstyrene, m-methylstyrene, 2,4-dimethylstyrene, 2,5-dimethylstyrene, 3,4-dimethylstyrene, 3,5-dimethylstyrene, p-tert-butylstyrene and other alkylstyrene; p-chlorostyrene, m-chlorostyrene, o-chlorostyrene, p-bromostyrene, m-bromostyrene, o-bromostyrene, p-fluorostyrene, m-fluorostyrene, o-fluorostyrene, o-methylp-fluorostyrene and other halogenated styrene; maleic anhydride, maleic acid, fumaric acid, allyl alcohol, 3-buten-2-ol, methylbuten-1-ol, vinyl acetate, vinyl chloride, etc.
[0195] The aforementioned monomers can be used alone or in combination of two or more.
[0196] Commercially available petroleum resins may be used appropriately, such as aliphatic petroleum resins like QUINTON A100, QUINTON B170, QUINTON K100, QUINTON M100, QUINTON R100, QUINTON C200S manufactured by NIPPON ZEON (stock), MAURKALETS T-100AS, MAURKALETS R-100AS manufactured by Maruzen Petrochemical (stock), and aromatic petroleum resins like NEOPOLYMER L-90, NEOPOLYMER 120, NEOPOLYMER 130, NEOPOLYMER 140, NEOPOLYMER 150, NEOPOLYMER 170S, NEOPOLYMER 160, NEOPOLYMER E-100, NEOPOLYMER E-130, NEOPOLYMER 130S, and NEOPOLYMER E-100. S. Tosoh Corporation's PETOCOL LX, PETOCOL LX-HS, PETOCOL 100T, PETOCOL 120, PETOCOL 120HS, PETOCOL 130, PETOCOL 140, PETOCOL 140HM, PETOCOL 140HM5, PETOCOL 150, PETOCOL 150AS, copolymerized petroleum resins, such as NIPPON ZEON Corporation's QUINTON D100, QUINTON N180, QUINTON P195N, QUINTON S100, QUINTON S195, QUINTON U185, QUINTON G100B, QUINTON G115, QUINTON D200, QUINTON E200SN, QUINTON N295, Tosoh Corporation's PETROTAC 60, PETROTAC 70, PETROTAC 90, PETROTAC 90V, PETROTAC 100, PETROTAC 100V, PETROTAC 90HM, DCPD (dicyclopentadiene) based petroleum resins, such as MAURKALETS M-890A and MAURKALETS M-845A manufactured by Maruzen Petrochemical Co., Ltd., QUINTON 1325, QUINTON 1345, QUINTON 1500, QUINTON 1525L, QUINTON 1700 manufactured by NIPPON ZEON Co., Ltd., and HA085, HA103, HA105, HA125, HB103, HB125, etc. manufactured by ENEOS Co., Ltd.Furthermore, petroleum resins may also be those described in Organic Synthetic Chemistry, Volume 25, No. 6 (1967).
[0197] When the resin composition of this embodiment contains petroleum resin, the lower limit of its content relative to 100 parts by mass of the resin solids in the resin composition is preferably 1 part by mass or more, more preferably 5 parts by mass or more, more preferably 10 parts by mass or more, more preferably 20 parts by mass or more, and ideally more than 25 parts by mass. By being above the aforementioned lower limit, the melt viscosity tends to decrease. Furthermore, the upper limit of the petroleum resin content relative to 100 parts by mass of the resin solids in the resin composition is preferably 70 parts by mass or less, more preferably 50 parts by mass or less, and 40 parts by mass or less is also acceptable. By being below the aforementioned upper limit, Df tends to decrease. The resin composition of this embodiment may contain only one type of petroleum resin, or it may contain two or more types. When containing two or more types, the total amount within the above range is preferred. Furthermore, the resin composition of this embodiment may also be substantially free of petroleum resin. "Not actually contained" means that the content of petroleum resin is less than 1 part by weight of the solid resin component in the resin composition, less than 0.1 parts by weight is better, and less than 0.01 parts by weight is even better.
[0198] <Filler (D)> The resin composition of this embodiment preferably contains filler (D). By containing filler (D), the low dielectric properties (Dk and / or Df), flame retardancy, and low thermal expansion of the resin composition and its cured form can be further improved. Furthermore, the filler (D) used in this embodiment is preferably superior in low dielectric properties (Dk and / or Df). For example, the relative permittivity (Dk) of the filler (D) used in this embodiment at a frequency of 10 GHz, measured by the cavity resonator perturbation method, is preferably 8.0 or less, more preferably 6.0 or less, and even more preferably 4.0 or less. Furthermore, a lower limit value of the relative permittivity, for example, 2.0 or more, is practical. Furthermore, the dielectric loss tangent (Df) of the filler (D) used in this embodiment at a frequency of 10 GHz, measured by the cavity resonator perturbation method, is preferably 0.05 or less, and more preferably 0.01 or less. Furthermore, the lower limit of the dielectric loss tangent, for example, above 0.0001, is the actual value.
[0199] The type of filler material (D) used in this embodiment is not particularly limited and can be ideally used by users of the art. Specifically, it includes, for example, silica-based materials such as natural silica, fused silica, synthetic silica, amorphous silica, aerosil, and hollow silica; metal oxides such as alumina, white carbon, titanium dioxide, titanium dioxide, zinc oxide, magnesium oxide, and zirconium oxide; composite oxides such as zinc borate, zinc stannate, forsterite, barium titanate, strontium titanate, and calcium titanate; nitrides such as boron nitride, condensed boron nitride, silicon nitride, and aluminum nitride; aluminum hydroxide; heat-treated aluminum hydroxide (aluminum hydroxide that has undergone heat treatment and reduced some of its water of crystallization); boehmite; and metal hydroxides (including hydrates) such as magnesium hydroxide. Inorganic fillers include molybdenum oxide, zinc molybdate and other molybdenum compounds, barium sulfate, clay, kaolin, talc, calcined clay, calcined kaolin, calcined talc, mica, E-glass, A-glass, NE-glass, NER-glass, C-glass, L-glass, D-glass, S-glass, M-glass G20, glass short fibers (including E-glass, T-glass, D-glass, S-glass, Q-glass and other glass micropowders), insulated glass, spherical glass, etc. Organic fillers include styrene-type, butadiene-type, acrylic-type rubber powders, core-shell rubber powders, polysiloxane resin powders, polysiloxane rubber powders, polysiloxane composite powders, etc. In this embodiment, inorganic fillers are preferred, and it is even more desirable to contain one or more of the following: silicon dioxide, aluminum hydroxide, aluminum nitride, boron nitride, magnesium olivine, titanium oxide, barium titanate, strontium titanate, and calcium titanate. Considering the low dielectric properties (Dk and / or Df), it is even more desirable to contain one or more of the following: silicon dioxide and aluminum hydroxide, with silicon dioxide being the most desirable component. By using such inorganic fillers, the heat resistance, low dielectric properties (Dk and / or Df), thermal expansion properties, dimensional stability, and flame retardancy of the cured resin composition are further improved.
[0200] In the resin composition of this embodiment, the content of filler (D) can be appropriately set according to the desired characteristics and is not particularly limited. It is preferable to have 10 parts by mass or more, more preferably 20 parts by mass or more, more preferably 40 parts by mass or more, more preferably 60 parts by mass or more, and ideally more than 80 parts by mass, relative to 100 parts by mass of the resin solids in the resin composition. By setting the content at or above the aforementioned lower limit, the heat resistance, low thermal expansion, and low dielectric loss tangent of the obtained cured product tend to be improved. Furthermore, the upper limit of the filler (D) content is preferable to be 1000 parts by mass or less, more preferably 500 parts by mass or less, more preferably 300 parts by mass or less, more preferably 250 parts by mass or less, and 200 parts by mass or less and 120 parts by mass or less, relative to 100 parts by mass of the resin solids. By setting the content at or below the aforementioned upper limit, the formability of the resin composition tends to be improved. In the resin composition of this embodiment, one ideal example is a sample in which the content of filler (D) is 30% to 90% by mass of the components other than the solvent. The resin composition of this embodiment may contain only one type of filler (D) or may contain two or more types. When containing two or more types, it is preferable that the total amount falls within the above-mentioned range.
[0201] In the resin composition of this embodiment, when filler (D) is used, especially inorganic filler, a silane coupling agent may also be included. By including a silane coupling agent, the dispersibility of filler (D) and the adhesive strength between the resin composition and filler (D) and the substrate described later tend to be improved. Silane coupling agents are not particularly limited, but examples include those used for surface treatment of common inorganic materials, such as aminosilane compounds (e.g., γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, etc.), epoxysilane compounds (e.g., γ-epoxypropoxypropyltrimethoxysilane, etc.), vinylsilane compounds (e.g., vinyltrimethoxysilane, etc.), styrylsilane compounds, acrylic silane compounds (e.g., γ-acryloxypropyltrimethoxysilane, etc.), cationic silane compounds (e.g., N-β-(N-vinylbenzylaminoethyl)-γ-aminopropyltrimethoxysilane hydrochloride, etc.), and phenylsilane compounds. Silane coupling agents can be used alone or in combination of two or more. The content of the silane coupling agent is not particularly limited, and it can be 0.1 to 5.0 parts by weight relative to 100 parts by weight of the resin solids.
[0202] <Monomers or oligomers having vinyl unsaturated groups> In the resin composition of this embodiment, monomers or oligomers having vinyl unsaturated groups may also be used to improve thermosetting properties and curing properties obtained by active energy rays (e.g., photocuring properties obtained by ultraviolet light). The use of oligomers or monomers having vinyl unsaturated groups in this embodiment is not particularly limited; for example, monomers or oligomers having vinyl, isopropenyl, allyl, (meth)acrylic, etc., are preferred, with vinyl monomers or oligomers being more desirable. Furthermore, in this specification, compounds that are monomers or oligomers having vinyl unsaturated groups and belong to the category of polyphenylene ether compounds (B) are referred to as polyphenylene ether compounds (B).
[0203] More specifically, a monomer having an ethylene unsaturated group, such as a compound (F1) (compound (F1)) with a molecular weight of less than 1,000 and containing one organic group containing an ethylene unsaturated bond. The ethylene unsaturated bond constituting the aforementioned organic group containing an ethylene unsaturated bond does not include ethylene unsaturated bonds contained as part of an aromatic ring. On the other hand, it includes ethylene unsaturated bonds contained as part of a non-aromatic ring. Examples of ethylene unsaturated bonds contained as part of a non-aromatic ring include cyclohexenyl groups in a molecule. Furthermore, it also includes portions other than the ends of straight-chain or branched organic groups, that is, ethylene unsaturated bonds contained in straight-chain or branched chains. The aforementioned organic group containing an ethylene unsaturated bond is preferably selected from the group consisting of vinyl, isopropenyl, allyl, acrylamide, and methacrylic acid groups, with vinyl being more preferred. Furthermore, in this specification, compounds that are monomers or oligomers having ethylene unsaturated groups and also belong to silane coupling agents are used as silane coupling agents.
[0204] The compound (F1) used in this embodiment is preferably composed only of atoms selected from carbon, hydrogen, oxygen, nitrogen, and silicon atoms; more preferably, it is composed only of atoms selected only from carbon, hydrogen, oxygen, and silicon atoms; and even more preferably, it is composed only of atoms selected only from carbon, hydrogen, oxygen, and oxygen atoms. The compound (F1) used in this embodiment may or may not have polar groups. The compound (F1) used in this embodiment preferably does not have polar groups. Polar groups include, for example, amino, carboxyl, hydroxyl, and nitro groups.
[0205] In this embodiment, it is preferable that the molecular weight of compound (F1) is 70 or higher, more preferably 80 or higher, and even more preferably 90 or higher. By having a molecular weight of 70 or higher than the aforementioned lower limit, there is a tendency to suppress the volatilization of compound (F1) from the resin composition and its cured products of this embodiment. It is preferable that the molecular weight of compound (F1) is 500 or lower, more preferably 400 or lower, more preferably 300 or lower, even more preferably 200 or lower, and 150 or lower is also acceptable. By having a molecular weight of 500 or lower than the aforementioned upper limit, there is a tendency to further enhance the reactivity with other resin components. When the resin composition of this embodiment contains two or more compounds (F1), it is preferable that the average molecular weight of the compounds (F1) is within the above-mentioned range, and it is even preferable that the molecular weight of each compound is within the above-mentioned ideal range.
[0206] In this embodiment, the boiling point of compound (F1) is preferably 110°C or higher, more preferably 115°C or higher, and even more preferably 120°C or higher. By having a boiling point of 110°C or higher than the aforementioned lower limit, the volatilization of compound (F1) during the thermosetting of the resin composition is suppressed, allowing other curing compounds (C) to react with compound (F1). The boiling point of the aforementioned compound (F1) is preferably 300°C or lower, more preferably 250°C or lower, and even more preferably 200°C or lower. By having a boiling point of 200°C or lower than the aforementioned upper limit, it is less likely to remain as a residual solvent in the cured product. When the resin composition of this embodiment contains two or more compounds (F1), it is acceptable as long as the average boiling point falls within the above range, but it is preferable that the boiling point of each compound is within the above ideal range.
[0207] Compound (F1), for example: unsaturated polyester compounds based on (meth)acrylate compounds, aromatic vinyl compounds (preferably styrene-based compounds), compounds containing isopropenyl groups, saturated fatty acid vinyl ester compounds, cyanide vinyl compounds, vinyl unsaturated carboxylic acids, vinyl unsaturated carboxylic anhydrides, vinyl unsaturated dicarboxylic acid monoalkyl esters, vinyl unsaturated carboxylamines, maleic anhydrides, fumaric acid, itaconic acid, and citraconic acid; unsaturated epoxy (meth)acrylate compounds containing acrylonitrile or methacrylonitrile; compounds containing vinyl or (meth)allyl groups. Unsaturated epoxy compounds, carbamate (meth)acrylate compounds, polyether (meth)acrylate compounds, polyol (meth)acrylate compounds, alkyd acrylate compounds, polyester acrylate compounds, spiroacetal acrylate compounds, diallyl phthalate compounds, diallyl tetrabromophthalate compounds, diethylene glycol dielyl carbonate, and polyethylene polythiols, preferably selected from at least one of the group consisting of (meth)acrylate compounds, aromatic vinyl compounds, and saturated fatty acid vinyl ester compounds, with aromatic vinyl compounds being more preferred. Specific examples of compound (F1) include methylstyrene (e.g., 4-methylstyrene), ethylvinylbenzene, diethyl-4-vinylbenzylphosphonate, 4-vinylbenzylepoxypropyl ether, α-methylstyrene, etc. Furthermore, specific examples of compound (F1) can be found in paragraphs 0046 and 0049 of Japanese Patent Application Publication No. 2019-194312, the contents of which are incorporated herein by reference.
[0208] On the other hand, in order to improve the low dielectric constant and low dielectric loss tangent, it is also desirable for the resin composition of this embodiment to contain a styrene oligomer (F2). The styrene oligomer (F2) of this embodiment is preferably formed by polymerizing styrene with at least one of the groups selected from styrene derivatives and vinyltoluene. The number average molecular weight of the styrene oligomer (F2) is preferably 178 or more, and more preferably 1600 or less. Furthermore, the styrene oligomer (F2) is preferably a compound with an average number of aromatic rings of 2 to 14, a total amount of 2 to 14 aromatic rings of 50% by mass or more, and a boiling point of 300°C or more, and has an unbranched structure.
[0209] The styrene oligomer (F2) used in this embodiment includes, for example, styrene polymers, vinyltoluene polymers, α-methylstyrene polymers, vinyltoluene-α-methylstyrene polymers, and styrene-α-styrene polymers. Commercially available styrene polymers may also be used, such as Piccotex A5 (manufactured by Eastman Chemical Company), Piccotex A-75 (manufactured by Eastman Chemical Company), Piccotex 75 (manufactured by Eastman Chemical Company), FTR-8100 (manufactured by Mitsui Chemicals), and FTR-8120 (manufactured by Mitsui Chemicals). Furthermore, examples of vinyltoluene-α-methylstyrene polymers include Piccotex LC (manufactured by Eastman Chemical Company). Furthermore, examples of α-methylstyrene polymers include: Crystalx 3070 (manufactured by Eastman Chemical Company), Crystalx 3085 (manufactured by Eastman Chemical Company), Crystalx (3100), Crystalx 5140 (manufactured by Eastman Chemical Company), FMR-0100 (manufactured by Mitsui Chemicals Co., Ltd.), and FMR-0150 (manufactured by Mitsui Chemicals Co., Ltd.). Also, examples of styrene-α-styrene polymers include: FTR-2120 (manufactured by Mitsui Chemicals Co., Ltd.). These styrene oligomers can be used alone or in combination of two or more. In the resin composition of this embodiment, the α-methylstyrene oligomer is more ideal due to its good thermosetting properties, excellent embedding properties for fine wiring and solder heat resistance, low relative permittivity, and excellent low dielectric loss tangent.
[0210] Furthermore, in the resin composition of this embodiment, it is also desirable to include a divinyl compound (F3) as a monomer with vinyl unsaturated groups in order to improve the low dielectric constant and low dielectric loss tangent. The divinyl compound is a low-molecular-weight compound having two vinyl groups. Because there are two vinyl groups, a good crosslinking density is achieved, resulting in an increase in the free volume of the molecule, thus suppressing the dielectric loss tangent (Df) of the obtained cured material to a small value. Moreover, it is believed that since the divinyl compound (F3) is used as a substitute for resin (A), polyphenylene ether compound (B), and other curing compounds, the reduction in the content of components with polar groups also contributes to the reduction of dielectric loss tangent (Df). Furthermore, because the divinyl compound has two vinyl functional groups, the reactivity between resin (A) and polyphenylene ether compound (B) becomes better, resulting in a tendency to easily improve heat resistance. Furthermore, the divinyl compounds (F3) mentioned here refer to those with a molecular weight of less than 600, preferably below 300, and even more preferably below 195. Also, the lower limit of 54 for molecular weight is an actual figure. Examples of divinyl compounds (F3) include divinylbenzene, 1-ethynyl-4-[2-(4-ethynylphenyl)ethyl]benzene (BVPE), and 1,3-vinyltetramethylsiloxane.
[0211] In addition, monomers or oligomers having vinyl unsaturated groups, such as 1,3-diisopropenylbenzene and 1,4-diisopropenylbenzene, are also preferred. Furthermore, details of monomers or oligomers having vinyl unsaturated groups can be found in paragraphs 0069 to 0087 of International Publication No. 2017 / 135168 and paragraphs 0065 to 0067 of International Publication No. 2019 / 230945, the contents of which are incorporated herein by reference.
[0212] When the resin composition of this embodiment contains monomers or oligomers having vinyl unsaturated groups, the content of such monomers or oligomers relative to 100 parts by mass of the resin solids in the resin composition is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, more preferably 2 parts by mass or more, more preferably 3 parts by mass or more, and 5 parts by mass or more is also acceptable. By reaching the aforementioned lower limit or above, the low dielectric properties (Dk and / or Df) of the obtained cured product tend to be further improved. Furthermore, the upper limit of the content of monomers or oligomers having vinyl unsaturated groups relative to 100 parts by mass of the resin solids in the resin composition is preferably 30 parts by mass or less, more preferably 25 parts by mass or less, more preferably 20 parts by mass or less, more preferably 15 parts by mass or less, and ideally 10 parts by mass or less. By reaching the aforementioned upper limit or below, the heat resistance of the obtained cured product tends to be further improved. Furthermore, the low dielectric constant, low dielectric loss tangent, and chemical resistance tend to be further improved. The resin composition of this embodiment may contain only one monomer or oligomer with an ethylene unsaturated group, or it may contain two or more. When it contains two or more, the total amount is preferably within the range described above.
[0213] <Flame Retardant> The resin composition of this embodiment may also contain a flame retardant. Flame retardants include, for example, phosphorus-based flame retardants, halogen-based flame retardants, inorganic flame retardants, and polysiloxane-based flame retardants, with phosphorus-based flame retardants being preferred. Known flame retardants may be used, such as: brominated epoxy resin, brominated polycarbonate, brominated polystyrene, brominated styrene, brominated phthalimide, tetrabromobisphenol A, pentabromobenzyl (meth)acrylate, pentabromotoluene, tribromophenol, hexabromobenzene, decabromodiphenyl ether, bis-1,2-pentabromophenylethane, chlorinated polystyrene, chlorinated paraffin, and other halogen-based flame retardants; red phosphorus, tricresyl phosphate, triphenyl phosphate, cresoldiphenyl phosphate, tri(xylene) phosphate, etc. Phosphorus-based flame retardants include trialkyl phosphate, dialkyl phosphate, ethyl chlorophosphate, phosphonocyanate, 1,3-epoxyphenylbis(2,6-di(xylyl)phosphate), and 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide; inorganic flame retardants include aluminum hydroxide, magnesium hydroxide, some boehmite, zinc borate, and antimony trioxide; and polysiloxane-based flame retardants include polysiloxane rubber and polysiloxane resin. In this embodiment, 1,3-epoxyphenylbis(2,6-di(xylyl)phosphate) is preferred because it does not impair the low dielectric properties (Dk and / or Df) of the resulting cured material.
[0214] When the resin composition of this embodiment contains a flame retardant, its content is preferably 1 part by weight or more, and more preferably 5 parts by weight or more, relative to 100 parts by weight of the solid resin component in the resin composition. Furthermore, the lower limit of the flame retardant content is preferably 30 parts by weight or less, and more preferably 25 parts by weight or less. One type of flame retardant may be used alone or in combination of two or more. When two or more are used, the total amount shall be within the above-mentioned range.
[0215] <Active Ester Compound> The resin composition of this embodiment may also contain an active ester compound. The active ester compound is not particularly limited, for example, see paragraphs 0064 to 0066 of International Publication No. 2021 / 172317, the contents of which are incorporated herein by reference.
[0216] When the resin composition of this embodiment contains an active ester compound, it is preferable that it is 1 part by mass or more relative to 100 parts by mass of the resin solids in the resin composition, and preferably 90 parts by mass or less, and 50 parts by mass or less is also acceptable. The resin composition of this embodiment may contain only one type of active ester compound, or it may contain two or more types. When it contains two or more types, it is preferable that the total amount falls within the above-mentioned range. Furthermore, the resin composition of this embodiment may also be substantially free of active ester compounds. "Substantially free" means that the content of the active ester compound relative to 100 parts by mass of the resin solids in the resin composition is less than 1 part by mass, less than 0.1 parts by mass is preferable, and less than 0.01 parts by mass is even more preferable.
[0217] <Dispersant> The resin composition of this embodiment may also contain a dispersant. The dispersant can ideally be any type commonly used in coating applications, and there are no particular limitations on its type. Copolymer-based wetting dispersants and fluorinated dispersants containing fluorine are preferred. Specific examples of dispersants include BYK Chemie Japan's DISPERBYK (registered trademark)-110, 111, 161, 180, 2009, 2152, 2155, BYK (registered trademark)-W996, W9010, W903, W940, NEOS's Ftergent, and Mitsubishi Pencil's MPT, etc.
[0218] When the resin composition of this embodiment contains a dispersant, the lower limit of its content relative to 100 parts by weight of the resin solids in the resin composition is preferably 0.01 parts by weight or more, more preferably 0.1 parts by weight or more, and 0.3 parts by weight or more is also acceptable. Furthermore, the upper limit of the dispersant content relative to 100 parts by weight of the resin solids in the resin composition is preferably 10 parts by weight or less, more preferably 5 parts by weight or less, and even more preferably 3 parts by weight or less. One type of dispersant may be used alone or in combination of two or more types. When two or more types are used, the total amount falls within the above-mentioned range.
[0219] <Curing Accelerator> The resin composition of this embodiment may further contain a curing accelerator. The curing accelerator is not particularly limited, and may include, for example: imidazoles such as 2-ethyl-4-methylimidazolium and triphenylimidazolium; organic peroxides such as benzoyl peroxide, bis(1-methyl-1-phenylethyl) peroxide, di-tert-butyl peroxide, lauryl peroxide, acetyl peroxide, p-chlorobenzoyl peroxide, di-tert-butyl ditert-phthalate, α,α'-di(tert-butylperoxide)diisopropylbenzene, 2,5-dimethyl-2,5-di(tert-butylperoxide)hexane, and 2,5-dimethyl-2,5-bis(tert-butylperoxide)hex-3-yne; azo compounds such as azobisnitrile (e.g., azobisisobutyronitrile); N,N-dimethylbenzylamine, N,N-dimethylaniline, and N,N-dimethyltoluidine. Tertiary amines such as 2-N-ethylaniline ethanol, tri-n-butylamine, pyridine, quinoline, N-methylphenyl cyanoline, triethanolamine, triethylenediamine, tetramethylbutanediamine, and N-methylpiperidine; phenols such as phenol, xylenol, cresol, resorcinol, and catechol; high-temperature decomposition free radical generators such as 2,3-dimethyl-2,3-diphenylbutane; organometallic salts such as lead naphthenate, lead stearate, zinc naphthenate, zinc octanoate, manganese octanoate, tin oleate, dibutyltin malate, manganese naphthenate, cobalt naphthenate, and acetylacetone iron; these organometallic salts dissolved in phenol, bisphenol, and other hydroxyl-containing compounds; inorganic metal salts such as tin chloride, zinc chloride, and aluminum chloride; organotin compounds such as dioctyltin oxide, other alkyltin compounds, and alkyltin oxides. The curing accelerator is preferably selected from at least one of the groups consisting of imidazoles, organic peroxides, and organometallic salts, with imidazoles and / or organometallic salts being more preferred, and a combination of imidazoles and organometallic salts being even better. Furthermore, in this embodiment, the composition may also be substantially free of polymerization initiators such as organic peroxides and azo compounds. "Substantially free" means that the content of the polymerization initiator relative to 100 parts by weight of the resin solids in the resin composition is less than 0.1 parts by weight, less than 0.01 parts by weight is preferred, and less than 0.001 parts by weight is even more preferred. In particular, when the polyphenylene ether compound represented by formula (OP-1) is used as the polyphenylene ether compound (B) with a terminal carbon-carbon unsaturated double bond, it can be sufficiently cured even if the composition is substantially free of polymerization initiators (including curing accelerators).
[0220] When the resin composition of this embodiment contains a curing accelerator, the lower limit of its content relative to 100 parts by weight of the resin solids in the resin composition is preferably 0.005 parts by weight or more, more preferably 0.01 parts by weight or more, and even more preferably 0.1 parts by weight or more. Furthermore, the upper limit of the curing accelerator content relative to 100 parts by weight of the resin solids in the resin composition is preferably 10 parts by weight or less, more preferably 5 parts by weight or less, and even more preferably 2 parts by weight or less. One type of curing accelerator may be used alone, or two or more may be used in combination. When two or more are used, the total amount falls within the above-mentioned range.
[0221] <Solvent> The resin composition of this embodiment may also contain a solvent, preferably an organic solvent. When containing a solvent, the resin composition of this embodiment is preferably at least a portion of the various resin solid components mentioned above and preferably in a form (solution or varnish) that is completely soluble in or compatible with the solvent. There are no particular limitations on the solvent, which can dissolve or be compatible with at least a portion, and preferably all, of the aforementioned resin solid components. Examples of polar or nonpolar organic solvents include: ketones (e.g., acetone, methyl ethyl ketone, methyl isobutyl ketone, etc.), cellulose (e.g., propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, etc.), esters (e.g., ethyl lactate, methyl acetate, ethyl acetate, butyl acetate, isoamyl acetate, ethyl lactate, methyl methoxypropionate, methyl hydroxyisobutyrate, etc.), and acetamides (e.g., dimethoxyacetamide, dimethylmethoxyacetamide, etc.). Examples of nonpolar organic solvents include: aromatic hydrocarbons (e.g., toluene, xylene, etc.). One solvent may be used alone or in combination of two or more. When two or more solvents are used, the total amount constitutes the range described above.
[0222] <Other Components> In addition to the above-mentioned components, the resin composition of this embodiment may also contain various polymeric compounds such as resin and its oligomers, and various additives. Examples of additives include: ultraviolet absorbers, antioxidants, photopolymerization initiators, fluorescent whitening agents, photosensitizers, dyes, pigments, tackifiers, flow modifiers, lubricants, defoamers, leveling agents, gloss agents, polymerization inhibitors, etc. These additives may be used individually or in combination of two or more. Furthermore, the resin composition of this embodiment may also be substantially free of polymerization inhibitors. "Substantially free" means that the resin composition does not contain polymerization inhibitors, or that the content of polymerization inhibitors in the resin composition relative to 100 parts by weight of the resin solids is, for example: less than 0.008 parts by weight, preferably less than 0.007 parts by weight, more preferably less than 0.001 parts by weight, and ideally less than 0.0001 parts by weight.
[0223] <Applications> The resin composition of this embodiment can be used to form a cured product. Specifically, the resin composition of this embodiment, as a material with low dielectric properties (Dk and / or Df), is ideally used as an insulating layer for printed circuit boards, a material for semiconductor packages, and is also ideally used as a resin composition for electronic materials. The resin composition of this embodiment is ideally used as a prepreg, a metal-clad laminate using a prepreg, a resin composite sheet, and a material for printed circuit boards.
[0224] The resin composition of this embodiment preferably has a minimum melt viscosity of 100,000 Pa·s or less, and more preferably 20,000 Pa·s or less. There is no particular limitation on the lower limit of the minimum melt viscosity; 10 Pa·s or more is practical. Such a low melt viscosity can be achieved by using resin (A) and a polymer having constituent units represented by formula (V). Furthermore, the resin composition of this embodiment preferably has a viscosity (minimum melting temperature + 10°C) ÷ minimum melt viscosity of 80 times or less, and more preferably 20 times or less. If the viscosity (minimum melting temperature + 10°C) ÷ minimum melt viscosity is low, the curing reaction will proceed gently, and there is a tendency to effectively suppress pore formation. The minimum melt viscosity was measured according to the method described in the examples below.
[0225] The minimum melting temperature of the resin composition in this embodiment is preferably below 210°C, more preferably below 200°C, more preferably below 190°C, even more preferably below 180°C, and ideally below 175°C. Lower limits, for example, above 120°C, are practical. The minimum melting temperature was determined according to the method described in the examples below.
[0226] The resin composition of this embodiment preferably has a glass transition temperature of 130°C or higher according to DMA (Dynamic Mechanical Analysis), more preferably 150°C or higher, more preferably 165°C or higher, even more preferably 170°C or higher, and 180°C or higher and 190°C or higher are also acceptable. This high glass transition temperature can be achieved by primarily using a polyphenylene ether compound (B). An upper limit for the glass transition temperature, for example, below 350°C, is practical. The glass transition temperature was measured according to the method described in the examples below.
[0227] In this embodiment, the relative permittivity (Dk) of the cured resin composition is preferably low. Specifically, a relative permittivity (Dk) of 2.50 or less at a frequency of 10 GHz, measured by the cavity resonator perturbation method, is preferably less than 2.45, and even more preferably less than 2.44. The lower limit of the relative permittivity (Dk) is not particularly limited; for example, 0.01 or more is practical. Furthermore, in this embodiment, the dielectric loss tangent (Df) of the cured resin composition is preferably low. Specifically, a dielectric loss tangent (Df) of 0.0022 or less at a frequency of 10 GHz, measured by the cavity resonator perturbation method, is preferably less than 0.0022, even more preferably less than 0.0021, even more preferably less than 0.0020, and also less than 0.0018, less than 0.0015, less than 0.0014, or less than 0.0013 is acceptable. The lower limit of the dielectric loss tangent (Df) is not particularly limited; for example, values above 0.0001 are practical. This low dielectric characteristic is primarily achieved by using a resin (A) and a polymer having constituent units represented by formula (V). The relative permittivity (Dk) and dielectric loss tangent (Df) are measured according to the methods described in the examples below.
[0228] The resin composition of this embodiment can be a layered material (including thin film and sheet types) such as a prepreg or resin composite sheet used as an insulating layer for a printed wiring board. When making such a layered material, its thickness is preferably 5 μm or more, and more preferably 10 μm or more. The upper limit of the thickness is preferably 200 μm or less, and more preferably 180 μm or less. In addition, the thickness of the aforementioned layered material, for example, when the resin composition of this embodiment is impregnated with glass cloth, refers to the thickness including the glass cloth. The material formed from the resin composition of this embodiment can be used for exposure and development to form patterns, and can also be used for applications without exposure and development. It is particularly suitable for applications without exposure and development.
[0229] <<Prepreg>> The prepreg system of this embodiment is formed from a substrate (prepreg substrate) and the resin composition of this embodiment. The prepreg of this embodiment can be obtained, for example, by applying the resin composition of this embodiment to the substrate (e.g., impregnating and / or coating) and then semi-curing it by heating (e.g., drying it at 120~220°C for 2~15 minutes). At this time, the amount of resin composition adhering to the substrate, that is, the amount of resin composition (including filler (D)) relative to the total amount of the semi-cured prepreg, is preferably in the range of 20~99% by mass, and more preferably in the range of 20~80% by mass.
[0230] There are no special restrictions on the substrate material if it is the same as the substrate material used in various printed wiring board materials. Examples of substrate materials include: glass fiber (e.g., E-glass, D-glass, L-glass, S-glass, T-glass, Q-glass, UN-glass, NE-glass, NER-glass, spherical glass, etc.), inorganic fibers other than glass (e.g., quartz, etc.), and organic fibers (e.g., polyimide, polyamide, polyester, liquid crystal polyester, polytetrafluoroethylene, etc.). The form of the substrate is not particularly limited, such as woven fabric, non-woven fabric, roving, woven felt, surface felt, etc. These substrate materials can be used individually or in combination of two or more. Among these substrates, considering dimensional stability, fabrics that have undergone superfiber opening and pore filling treatments are preferable. Considering strength and low water absorption, glass fabrics with a substrate thickness of 200 μm or less and a mass of 250 g / m² or less are preferable. Considering moisture absorption and heat resistance, glass fabrics that have undergone surface treatment using silane coupling agents such as epoxy silanes and amino silanes are preferable. Considering electrical properties, low-dielectric glass cloths composed of glass fibers exhibiting low relative permittivity and low dielectric loss tangent, such as L-glass, NE-glass, NER-glass, and Q-glass, are more preferred. Substrates with low relative permittivity include, for example, substrates with a relative permittivity of 5.0 or less (preferably 3.0 to 4.9). Substrates with low dielectric loss tangent include, for example, substrates with a dielectric loss tangent of 0.006 or less (preferably 0.001 to 0.005). The relative permittivity and dielectric loss tangent were measured using a cavity resonator at a frequency of 10 GHz using the perturbation method.
[0231] <<Metal-coated Foil Laminate>> The metal-coated foil laminate of this embodiment includes at least one layer formed from the prepreg of this embodiment, and metal foil disposed on one or both sides of the layer formed from the aforementioned prepreg. A method for manufacturing the metal-coated foil laminate of this embodiment can be exemplified by, for example, a method of stacking at least one (preferably two or more overlapping) prepreg of this embodiment, and then stacking it after placing metal foil on one or both sides. More specifically, it can be manufactured by stacking copper, aluminum, or other metal foils on one or both sides of the prepreg. The number of prepreg sheets is preferably 1 to 10, more preferably 2 to 10, and even more preferably 2 to 9. If the metal foil is a material used for printed circuit boards, there are no particular limitations; examples include, rolled copper foil, electrolytic copper foil, and other copper foils. The thickness of the metal foil (preferably copper foil) is not particularly limited and can be approximately 1.5 to 70 μm. Furthermore, when using copper foil as the metal foil, the surface roughness Rz of the copper foil should be adjusted to be 0.2~4.0 μm, as measured according to JIS B0601:2013. Adjusting the surface roughness Rz of the copper foil to 0.2 μm or higher tends to achieve an appropriate surface roughness and further improve the peel strength of the copper foil. On the other hand, adjusting the surface roughness Rz of the copper foil to 4.0 μm or lower tends to achieve an appropriate surface roughness and further improve the dielectric loss tangent. Considering the reduction of dielectric loss tangent, a surface roughness Rz of 0.5 μm or higher is preferred, 0.6 μm or higher is even better, 0.7 μm or higher is particularly good, and 3.5 μm or lower is preferred, 3.0 μm or lower is even better, and 2.0 μm or lower is particularly good.
[0232] Methods for lamination forming include those commonly used when forming laminated boards and multilayer boards for printed circuit boards. More specifically, methods using multilayer presses, multilayer vacuum presses, continuous forming machines, and autoclave forming machines, with lamination forming at temperatures of approximately 180-350°C, heating times of approximately 100-300 minutes, and surface pressures of approximately 20-100 kg / cm², can be listed. Alternatively, a multilayer board can be manufactured by combining the prepreg of this embodiment with a separately manufactured inner layer circuit board and laminating them. For example, a method for manufacturing a multilayer board can be achieved by depositing approximately 35 μm copper foil on both sides of a prepreg of this embodiment, laminating it using the above forming method to form an inner layer circuit, applying a blackening treatment to the circuit to form an inner layer circuit board, then alternately depositing the inner layer circuit board and the prepreg of this embodiment one by one, depositing copper foil on the outermost layer, and laminating it under vacuum conditions as described above to manufacture the multilayer board. The metal foil laminate of this embodiment can be ideally used as a printed wiring board.
[0233] As described above, the resin composition for electronic materials obtained by using the resin composition of this embodiment (a resin composition composed of a combination of specific components) can be characterized by the formability of the resin composition, the low dielectric properties (Dk and / or Df, especially low dielectric loss tangent) of its cured product, as well as the low relative permittivity, crack resistance, appearance of the cured product, low thermal expansion, and excellent moisture absorption and heat resistance.
[0234] <<Printed Wiring Board>> The printed wiring board of this embodiment includes an insulating layer and a conductor layer disposed on the surface of the aforementioned insulating layer. The aforementioned insulating layer includes at least one of a layer formed by the resin composition of this embodiment and a layer formed by the prepreg of this embodiment. Such a printed wiring board can be manufactured according to common methods, and there are no particular limitations on the manufacturing method. The following is an example of a method for manufacturing a printed wiring board. First, a copper-clad laminate or a metal-clad laminate is prepared. Then, the surface of the metal-clad laminate is etched to form the inner layer circuit, and an inner layer substrate is made. The surface of the inner layer circuit of the inner layer substrate is subjected to a surface treatment to improve the adhesion strength as needed. Then, the required number of the aforementioned prepregs are stacked on the surface of the inner layer circuit, and then the metal foil for the outer layer circuit is stacked on the outside. Finally, it is heated and pressed to form a whole. In this manner, a multilayer laminate is manufactured in which an insulating layer composed of a substrate and a hardened resin is formed between the metal foils used for inner and outer layer circuits. Then, after drilling holes for through holes and vias into the multilayer laminate, a plated metal film is formed on the wall surface of the holes to conduct the metal foils used for inner and outer layer circuits. Finally, the metal foils used for outer layer circuits are etched to form the outer layer circuits, thereby manufacturing a printed wiring board.
[0235] The printed wiring board obtained in the above-described manufacturing example has an insulating layer and a conductor layer formed on the surface of the insulating layer, and the insulating layer is composed of the resin composition and / or its cured form as described in this embodiment. That is, the prepreg of this embodiment (e.g., a prepreg formed from a substrate and the resin composition of this embodiment impregnated or coated thereon) and the layer formed from the resin composition of the metal foil laminate of this embodiment become the insulating layer of this embodiment. Furthermore, this embodiment also relates to a semiconductor device containing the aforementioned printed wiring board. For details of the semiconductor device, please refer to paragraphs 0200 to 0202 of Japanese Patent Application Publication No. 2021-021027, and these contents are incorporated herein by reference.
[0236] Furthermore, the insulating layer formed from the hardened resin composition of this embodiment should preferably have a reduced surface roughness after roughening treatment. Specifically, the arithmetic mean roughness Ra of the surface of the roughened insulating layer should preferably be 200 nm or less, more preferably 150 nm or less, and especially preferably 100 nm or less. There is no particular limitation on the lower limit of the arithmetic mean roughness Ra, for example, it can be 10 nm or more. The arithmetic mean roughness Ra of the surface of the insulating layer is measured using a non-contact surface roughness meter in VSI mode with a 50x lens. The non-contact surface roughness meter used is a Veeco Instruments WYKONT3300.
[0237] <<Resin Composite Sheet>> The resin composite sheet of this embodiment includes a support and a layer formed of the resin composition of this embodiment disposed on the surface of the aforementioned support. The resin composite sheet can be used as a film for deposition or a dry film solder resist. There are no particular limitations on the manufacturing method of the resin composite sheet, and examples include methods such as coating a solution obtained by dissolving the resin composition of this embodiment in a solvent onto a support and then drying it to obtain the resin composite sheet.
[0238] Examples of supports used herein include: polyethylene film, polypropylene film, polycarbonate film, polyethylene terephthalate film, ethylene tetrafluoroethylene copolymer film, and release films formed by coating the surface of these films with a release agent, organic film substrates such as polyimide film, conductor foils such as copper foil and aluminum foil, glass plates, SUS (Steel Use Stainless) plates, FRP (Fiber-Reinforced Plastics) plates, etc., without particular limitation.
[0239] Coating methods (coating methods) can include, for example, applying a solution obtained by dissolving the resin composition of this embodiment in a solvent onto a support using a coating rod, a die coater, a doctor blade, or a Baker applicator. Alternatively, a single-layer sheet can be formed by peeling or etching the support from a resin composite sheet formed by laminating the support and the resin composition after drying. Furthermore, a single-layer sheet can be obtained without using a support by supplying a solution obtained by dissolving the resin composition of this embodiment in a solvent into a mold having a sheet-like mold groove and drying it.
[0240] Furthermore, when manufacturing the single-layer sheet or resin composite sheet of this embodiment, there are no particular restrictions on the drying conditions for removing the solvent. At low temperatures, solvent may remain in the resin composition; at high temperatures, the resin composition will harden. Therefore, drying at a temperature of 20°C to 200°C for 1 to 90 minutes is preferable. Also, the single-layer sheet or resin composite sheet can be used in its uncured state after only the solvent has been dried, or it can be used in a semi-cured (B-stage) state as needed. In addition, the thickness of the resin layer in the single-layer sheet or resin composite sheet of this embodiment can be adjusted by the concentration of the resin composition solution of this embodiment used during coating (coating) and the coating thickness, and there are no particular restrictions. Generally speaking, if the coating thickness is too thick, solvent may remain during drying; therefore, a thickness of 0.1 to 500 μm is preferable. [Example]
[0241] The present invention will be described more specifically below with examples. The materials, amounts, proportions, processing contents, and processing procedures shown in the following examples may be appropriately modified without departing from the concept of the present invention. Therefore, the scope of the present invention is not limited to the specific examples shown below. When the measuring equipment used in the examples is not readily available due to production stoppages, other equipment with equivalent performance may be used for measurement.
[0242] <Determination of Weight Average Molecular Weight and Number Average Molecular Weight> The weight average molecular weight (Mw) and number average molecular weight (Mn) of a resin (A) with terminal groups represented by formula (T1) and a dihydroindene backbone, a polyphenylene ether compound (B) with terminal carbon-carbon unsaturated double bonds, and a polymer with constituent units represented by formula (V) were determined by gel permeation chromatography (GPC). A delivery pump (Shimadzu Corporation, LC-20AD), a differential refractive index detector (Shimadzu Corporation, RID-10A), and GPC columns (Showa Denko Corporation, GPC KF-801, 802, 803, 804) were used. Tetrahydrofuran was used as the solvent at a flow rate of 1.0 mL / min, the column temperature was 40 °C, and a calibration curve made of monodisperse polystyrene was used.
[0243] <Determination of parameters α and β> The parameters α and β of resin (A) were calculated by 1H-NMR determination. The synthesized resin was dissolved in a mixed solvent of heptane and methanol and dried. This operation was repeated to remove residual solvent contained in the recovered solid. Then, the recovered solid was dissolved in CDCl3 and 1H-NMR was performed. In the 1H-NMR determination, the parameters α and β of each resin were calculated using the following formulas. [Formula 2] Parameter α (α) Parameter β (β) The values in parentheses in formulas (α) and (β) represent the integral values between the corresponding chemical shift values in 1H-NMR.
[0244] <Synthesis Example 1: Synthesis of Resin (A) with a terminal group represented by formula (T1) and a dihydroindene skeleton> 520 g of toluene, 3 g of activated clay, and a stir bar were placed in a three-necked flask equipped with a thermometer and a cooling tube. While stirring, the mixture was heated to an internal temperature of 70°C. Then, 150 g of 1,3-diisopropenylbenzene (manufactured by Tokyo Chemical Co., Ltd.) was added dropwise, controlling the dropwise rate so that the internal temperature did not exceed 80°C. After the addition, the mixture was stirred until the internal temperature dropped to 70°C. Then, another 150 g of 1,3-diisopropenylbenzene (manufactured by Tokyo Chemical Co., Ltd.) was added dropwise. After the addition was complete, the mixture was allowed to react for another 2 hours. At the end of the reaction, 433 g of toluene was added, and the activated clay was removed by filtration. The solvent was distilled off the filtrate under heating and reduced pressure to obtain 231 g of solid resin. The obtained resin (A) has a Mw of 2674, a Mn of 1153, and a Mw / Mn ratio of 2.3. In formula (Tx), the parameters α and β are 0.71, β and n+o+p are 6.3. The structures within parentheses in (a), (b), and (c) all have the same molecular weight. Assuming the Mn of the synthesized resin is the average molecular weight, n+o+p is calculated. Furthermore, GPC analysis confirms that the residual monomer is less than 1% by mass. The NMR spectrum of the obtained resin is shown in Figure 1.
[0245] <Synthesis Example 2 Polyphenylene ether compound (B) with carbon-carbon unsaturated double bonds at the ends> <<Synthesis of 2-functionalized polyphenylene ether oligomers>> In a 12L longitudinal reactor equipped with a stirrer, thermometer, air inlet pipe, and baffle, CuBr was charged 29.64 g (43.2 mmol), 1.86 g (10.8 mmol) of N,N'-di-tert-butylethylenediamine, 69.83 g (690.1 mmol) of n-butyldimethylamine, and 2,600 g of toluene were stirred at a reaction temperature of 40 °C. While mixing nitrogen and air to adjust the oxygen concentration to 8% by volume, a mixed gas was bubbled at a flow rate of 5.2 L / min. A mixed solution of 129.3 g (0.48 mol) of 2,2',3,3',5,5'-hexamethyl-(1,1'-biphenol)-4,4'-diol, 878.4 g (7.2 mol) of 2,6-dimethylphenol, 1.26 g (7.3 mmol) of N,N'-di-tert-butylethylenediamine, and 27.19 g (268.7 mmol) of n-butyldimethylamine was added dropwise over 230 minutes, with stirring. After the addition was complete, 1,500 g of an aqueous solution containing 48.06 g (126.4 mmol) of tetrasodium ethylenediaminetetraacetate was added to stop the reaction. The aqueous and organic layers were separated. The organic layer was washed with 1N hydrochloric acid aqueous solution and then with pure water. The obtained solution was concentrated to 50% by mass using an evaporator to obtain 1980 g of a toluene solution of a difunctional phenylene ether oligomer (resin "B0"). The number average molecular weight of resin "B0" converted from polystyrene by GPC was 2100, the weight average molecular weight of polystyrene converted from polystyrene by GPC was 3740, and the hydroxyl equivalent was 1070.
[0246] <<Synthesis of Modified Polyphenylene Ether Compounds>> 792 g of a 50% by mass toluene solution of a difunctional polyphenylene ether oligomer (BO) was dried in an evaporator, and 2772 g of N,N-dimethylacetamide was added. The mixture was concentrated until the solid content was 20% by mass, yielding 1980 g of a 79.80% by mass N,N-dimethylacetamide and 0.20% by mass toluene solution (BO) of the difunctional polyphenylene ether oligomer. Then, in a reactor equipped with a stirrer, thermometer, and reflux pipe, 1980 g of the difunctional polyphenylene ether oligomer solution (BO) (0.37 mol by OH equivalent) and 67.78 g (0.44 mol) of chloromethylstyrene (CMS-P) were fed and heated and stirred at 50°C. Maintaining the reaction temperature at 50℃, 84.48 g (0.44 mol) of a methanol solution of sodium methoxide (concentration: 28.4% by mass) was added dropwise, and the mixture was stirred for 1 hour. Then, 9.75 g (0.05 mol) of a methanol solution of sodium methoxide (concentration: 28.4% by mass) was added dropwise, and the mixture was stirred for 2 hours. Afterward, 5.91 g (0.05 mol) of an 85% by mass phosphoric acid aqueous solution was added to remove the generated inorganic salts. The reaction solution was then added dropwise to 1975 g of water to solidify it. Solid-liquid separation was performed using a centrifuge, followed by washing with pure water and methanol, and then drying under reduced pressure to obtain 381.87 g of the desired polyphenylene ether compound (B). The modified polyphenylene ether compound, measured by GPC, had a number average molecular weight of 2350, a weight average molecular weight of 3880, and a vinyl equivalent of 1220 g / vinyl.
[0247] <Synthesis Example 3: Synthesis of a polymer (va) having constituent units represented by formula (V)> 2.25 mol (292.9 g) of divinylbenzene, 1.32 mol (172.0 g) of ethylvinylbenzene, 11.43 mol (1190.3 g) of styrene, and 15.0 mol (1532.0 g) of n-propyl acetate were added to a reactor. 600 mmol of a boron trifluoride diethyl ether complex was added at 70°C, and the reaction was allowed to proceed for 4 hours. After stopping the polymerization reaction with an aqueous sodium bicarbonate solution, the oil layer was washed three times with pure water, and the polymer (va) having constituent units represented by formula (V) was recovered by devolatilization under reduced pressure at 60°C. The obtained polymer (va) having constituent units represented by formula (V) was weighed, confirming that 860.8 g of polymer (va) having constituent units represented by formula (V) was obtained.
[0248] The polymer (va) having constituent units represented by formula (V) obtained had a number average molecular weight Mn of 2,060, a weight average molecular weight Mw of 30,700, and a monodispersity Mw / Mn of 14.9. Resonance lines from each monomer unit used as a raw material were observed in the polymer (va) having constituent units represented by formula (V) by 13C-NMR and 1H-NMR analysis. Based on the NMR and GC analysis results, the proportion of each monomer unit (from each raw material) in the polymer (va) having constituent units represented by formula (V) was calculated as follows. Constituent units from divinylbenzene: 20.9 mol% (24.3 wt%) Constituent units from ethylvinylbenzene: 9.1 mol% (10.7 wt%) Constituent units from styrene: 70.0 mol% (65.0 wt%) Also, constituent units with residual vinyl groups from divinylbenzene: 16.7 mol% (18.5 wt%).
[0249] Example 1: 20 parts by mass of resin (A) obtained in Synthesis Example 1, 40 parts by mass of polyphenylene ether compound (B) with carbon-carbon unsaturated double bonds at the ends obtained in Synthesis Example 2, and 40 parts by mass of polymer (va) having the constituent unit represented by formula (V) obtained in Synthesis Example 3 were dissolved in methyl ethyl ketone and toluene and mixed to obtain a varnish. The blending amounts of the above components represent values based on the amount of solid components.
[0250] <Preparation of Test Pieces of Hardened Boards with a Thickness of 1.0 mm> The solvent was evaporated and distilled off from the obtained varnish to obtain resin composition powder. Using the obtained resin composition powder, hardened boards were prepared as follows: 4.5 g of resin composition powder was applied to a stainless steel mold with a height of 100 mm × 30 mm × 1.0 mm, and the mold was installed in a vacuum press (manufactured by Kitagawa Seiki Co., Ltd.) and pressed at 200°C for 1.5 hours with a surface pressure of 1.9 MPa. Using the obtained resin composition powder or hardened boards, the following were evaluated: minimum melt viscosity, viscosity (minimum melt temperature + 10°C) ÷ minimum melt viscosity, formability, minimum melt temperature, glass transition temperature, relative permittivity (Dk), and dielectric loss tangent (Df). The evaluation results are shown in Table 1.
[0251] <Determination and Evaluation Methods> (1) Minimum Melt Viscosity and Viscosity (Minimum Melting Temperature + 10°C) ÷ Minimum Melt Viscosity The resin composition powders obtained in each example and comparative example were tested by GC (GC-2025, manufactured by Shimadzu Corporation) to confirm that the residual solvent content was 1% by mass. 1g was taken and formed into tablets with a diameter of 25mm to prepare a test sample. The minimum melt viscosity (Pa・s) and viscosity (min・10°C) were determined using a viscoelasticity measuring device (ARES-G2, manufactured by TA INSTRUMENT Corporation) at a heating temperature of 2°C / min and a frequency of 10rad / s. The minimum melt viscosity was evaluated as follows. A: Below 20,000 Pa·s B: Above 20,000 Pa·s but below 100,000 Pa·s C: Above 100,000 Pa·s Also, calculate the viscosity (minimum melting temperature + 10°C) ÷ minimum melt viscosity. Evaluate as follows: A: Below 20 times B: Above 20 times but below 80 times C: Above 80 times
[0252] (2) Formability Formability is evaluated as follows. A: The evaluation result of the minimum melt viscosity and the value of viscosity (minimum melt viscosity + 10°C) ÷ minimum melt viscosity is A. B: The evaluation result of the minimum melt viscosity and the value of viscosity (minimum melt viscosity + 10°C) ÷ minimum melt viscosity is A or B, and at least one of them is B. C: The evaluation result of the minimum melt viscosity and the value of viscosity (minimum melt viscosity + 10°C) ÷ minimum melt viscosity includes C.
[0253] (3) The temperature at which the minimum melting temperature reaches the minimum melting viscosity is defined as the minimum melting temperature.
[0254] (4) Glass transition temperature: The glass transition temperature is determined using a dynamic viscoelasticity measuring device according to JIS C6481 5.17.2 and the DMA (Dynamic Mechanical Analysis) bending method for samples where the aforementioned hardened plate has been reduced to 12.7 mm × 30 mm. The peak temperature of the obtained loss modulus of elasticity is defined as the glass transition temperature. The unit is expressed in °C. The dynamic viscoelasticity measuring device used is a DMA Q800 manufactured by TA INSTRUMENT.
[0255] (5) Relative permittivity (Dk) and dielectric loss tangent (Df) After reducing the size of the aforementioned hardened board to 1.0 mm in width, it was dried at 120°C for 60 minutes. The relative permittivity (Dk) and dielectric loss tangent (Df) after drying were measured at 10 GHz using a perturbation method cavity resonator. The measurement temperature was set to 23°C. The perturbation method cavity resonator used was an Agilent 8722ES manufactured by Agilent Technologies.
[0256] Example 2 In Example 1, the content of resin (A) was changed to 25 parts by mass, the content of polyphenylene ether compound (B) was changed to 50 parts by mass, and the content of polymer (va) having the constituent unit represented by formula (V) was changed to 25 parts by mass, and otherwise the same procedure was followed.
[0257] Comparative Example 1 In Example 1, resin (A) and polymer (va) having constituent units represented by formula (V) were not used, and the content of polyphenylene ether compound (B) was changed to 100 parts by mass, otherwise the same procedure was followed.
[0258] Comparative Example 2 In Example 1, resin (A) and polyphenylene ether compound (B) were not used, and the content of polymer (va) having the constituent unit represented by formula (V) was changed to 100 parts by mass, otherwise the same procedure was followed.
[0259] [Table 1] unit Example 1 Example 2 Comparative Example 1 Comparative Example 2 Minimum melt viscosity Pa・s 1280 2030 22,800 17 - A A B A Viscosity of (minimum melting temperature + 10°C) ÷ Minimum melt viscosity - A A A C Formability - A A B C minimum melting temperature ℃ 160 163 169 148 Tg(DMA) ℃ 182 167 210 128 Dk @10GHz - 2.36 2.35 2.42 2.38 Df @10GHz - 0.0010 0.0012 0.0022 0.0009 [Simplified Explanation of the Diagram]
[0009] Figure 1 shows the NMR spectrum of Synthesis Example 1.
Claims
1. A resin composition comprising, relative to 100 parts by weight of a resin (A) having a dihydroindene backbone, 10-300 parts by weight of a polyphenylene ether compound (B) having terminal carbon-carbon unsaturated double bonds, and 10-300 parts by weight of a polymer having constituent units represented by formula (V), wherein the resin (A) is a resin represented by formula (T1-1), the number average molecular weight (Mn) of the resin (A) is 400-3000, the polymer having constituent units represented by formula (V) contains 3-90 mol% of constituent units derived from divinylbenzene and 10-90 mol% of constituent units derived from monovinyl aromatic compounds, and the number average molecular weight (Mn) of the polymer having constituent units represented by formula (V) is 300-130,000. In formula (T1-1), R is a base containing the constituent unit represented by formula (Tx), Mb independently represents a hydrocarbon group with 1 to 12 carbon atoms that can be substituted by halogen atoms, and y is an integer from 0 to 4. In formula (Tx), n, o, and p are the average number of repeating units, n represents a number greater than 0 and less than 20, o and p independently represent numbers from 0 to 20, 1.0≦n+o+p≦20.0, Ma independently represents a hydrocarbon group with 1 to 12 carbon atoms that can be substituted by halogen atoms, and x represents an integer from 0 to 4. Constituent units (a), (b), and (c) are bonded by * and constituent units (a), (b), (c), or other groups, respectively. Constituent units can also be bonded randomly. In formula (V), Ar represents an aromatic hydrocarbon linking group, and * represents the bonding position.
2. The resin composition as claimed in claim 1, wherein, The polyphenylene ether compound (B) with a carbon-carbon unsaturated double bond at the end contains a polyphenylene ether compound represented by formula (OP). In formula (OP), X represents an aromatic group, -(YO)n1- represents a polyphenylene ether structure, n1 represents an integer from 1 to 100, n2 represents an integer from 1 to 4, and Rx is a group represented by formula (Rx-1) or formula (Rx-2). In formulas (Rx-1) and (Rx-2), R1, R2, and R3 each independently represent a hydrogen atom, alkyl, alkenyl, or alkynyl group, * represents the bonding site with an oxygen atom, Mc each independently represents a hydrocarbon group with 1 to 12 carbon atoms, z represents an integer from 0 to 4, and r represents an integer from 1 to 6.
3. The resin composition as claimed in claim 1 or 2, wherein, The polyphenylene ether compound (B) with carbon-carbon unsaturated double bonds at the end contains a polyphenylene ether compound represented by formula (OP-1), in which X represents an aromatic group, -(YO)n2- represents a polyphenylene ether structure, R1, R2, and R3 each independently represent a hydrogen atom, alkyl, alkenyl, or alkynyl group, n1 represents an integer from 1 to 6, n2 represents an integer from 1 to 100, and n3 represents an integer from 1 to 4.
4. The resin composition as claimed in claim 1 or 2, wherein, The polyphenylene ether compound (B) with carbon-carbon unsaturated double bonds at the end has a number average molecular weight (Mn) of 500-3000 and a weight average molecular weight (Mw) of 800-6000.
5. The resin composition as claimed in claim 1 or 2, wherein, The mass ratio of resin (A) is 10 to 50 parts by mass relative to a total of 100 parts by mass of the resin (A) and the polyphenylene ether compound (B) with carbon-carbon unsaturated double bonds at the end.
6. The resin composition of claim 1 or 2 does not substantially contain polymerization inhibitors.
7. The resin composition of claim 1 or 2 further comprises the resin (A), the polyphenylene ether compound (B) having carbon-carbon unsaturated double bonds at the ends, and other compounds (C) besides the polymer having a constituent unit represented by formula (V).
8. The resin composition as claimed in claim 7, wherein, The other compound (C) contains one or more compounds selected from the group consisting of maleimide compounds, cyanate compounds, epoxy compounds, phenolic compounds, compounds containing (meth)allyl groups, oxetane resins, benzo[a]benzene compounds, arylcyclobutene resins, polyamide resins, polyimide resins, perfluoroethylene ether resins, styrene compounds other than the polyphenylene ether compound (B) with a carbon-carbon unsaturated double bond at the end, isopropylene compounds other than the resin (A) with a dihydroindene skeleton, polyfunctional (meth)acrylate compounds other than the polyphenylene ether compound (B) with a carbon-carbon unsaturated double bond at the end, elastomers, and petroleum resins.
9. The resin composition as claimed in claim 1 or 2, wherein, The total content of the resin (A) and the polyphenylene ether compound (B) with carbon-carbon unsaturated double bonds at the end is 40 parts by mass or more, relative to 100 parts by mass of the resin solids in the resin composition.
10. The resin composition of claim 1 or 2 further includes filler (D).
11. The resin composition as claimed in claim 10, wherein, The content of filler (D) is 10 to 1000 parts by mass relative to 100 parts by mass of the resin solids in the resin composition.
12. The resin composition as claimed in claim 1, wherein, The polyphenylene ether compound (B) with terminal carbon-carbon unsaturated double bonds contains a polyphenylene ether compound represented by formula (OP-1). The number average molecular weight (Mn) of the polyphenylene ether compound (B) with terminal carbon-carbon unsaturated double bonds is 500-3000 and the weight average molecular weight (Mw) is 800-6000. The mass ratio of resin (A) to 100 parts by mass of the total of resin (A) and polyphenylene ether compound (B) with terminal carbon-carbon unsaturated double bonds is 10-50 parts by mass. It substantially does not contain polymerization inhibitors. The total content of resin (A) and polyphenylene ether compound (B) with terminal carbon-carbon unsaturated double bonds is 40 parts by mass or more, relative to 100 parts by mass of the resin solids component in the resin composition. In formula (OP-1), X represents an aromatic group, -(YO)n2- represents a polyphenylene ether structure, R1, R2, and R3 each independently represent a hydrogen atom, alkyl, alkenyl, or alkynyl group, n1 represents an integer from 1 to 6, n2 represents an integer from 1 to 100, and n3 represents an integer from 1 to 4.
13. A cured form of a resin composition as claimed in claims 1, 2 or 12.
14. A prepreg formed of a substrate and a resin composition as claimed in claims 1, 2 or 12.
15. A metal foil laminate comprising at least one layer formed of a prepreg as claimed in claim 14, and a metal foil disposed on one or both sides of the layer formed of the prepreg.
16. A resin composite sheet comprising a support and a layer disposed on the surface of the support, formed of a resin composition as claimed in claims 1, 2 or 12.
17. A printed wiring board comprising an insulating layer and a conductor layer disposed on the surface of the insulating layer, the insulating layer comprising a layer formed of a resin composition as claimed in claims 1, 2 or 12.
18. A semiconductor device comprising a printed wiring board as claimed in claim 17.
Citation Information
Patent Citations
Curable resin composition
CN1914239B
Production of high polymer of diisopropenylbenzene
JP1984145207A
Cross-linking auxiliary for thermoplastic elastomer and production of thermoplastic elastomer using the same
JP1994087962A
Curable resin composition, prepreg, metal-clad laminate, printed wiring board
JP2020105352A