Method for forming a part by inserting a solid-state metal alloy into a casting stack
By inserting metal alloys in a solid state into a casting stack for liquefaction within a furnace, the method addresses safety and quality issues in lost wax casting, facilitating the production of high-quality multi-material parts.
Patent Information
- Application Number
- US19/132508
- Authority / Receiving Office
- US · United States
- Patent Type
- Applications(United States)
- Current Assignee / Owner
- Priority Date
- 2022-11-25
- Filing Date
- 2023-11-23
- Publication Date
- 2026-11-19
AI Technical Summary
Existing lost wax casting methods face safety risks and quality challenges, particularly in forming bi-material parts due to the need for multiple pours and handling liquid metal alloys, which can lead to oxidation, thermal gradients, and operator hazards.
A method involving the insertion of metal alloys in a solid state into a casting stack, followed by liquefaction within the furnace, eliminating the need for pouring and allowing controlled solidification, thereby reducing safety risks and improving the quality of multi-material parts.
This approach simplifies the casting process, enhances safety by avoiding liquid metal handling, reduces scrap rates, and enables precise control over multi-material part formation, particularly in turbomachine blades.
Smart Images

Figure US20260364672A1-D00000_ABST
Abstract
Description
TECHNICAL FIELD
[0001] This disclosure relates to a method for forming a metal part by a lost wax casting method.
[0002] A method is particularly suitable for forming blades for aircraft turbomachines. The formed blades can be bi-material.PRIOR ART
[0003] Generally, known methods for forming parts using lost wax casting methods involve pouring a liquid metal alloy into the crucible of a ceramic casting stack. This step typically takes place in a furnace. The metal alloy then fills one or more molds within the casting stack. The assembly is then cooled to solidify the metal alloy, thereby forming a casting.
[0004] In order to improve the quality of the resulting part, it is preferable to perform the pouring under vacuum to avoid any unwanted reaction, for example oxidation of the metal alloy in the liquid state. Furthermore, the pouring is optimized independently for each metal alloy, since each metal alloy has different properties (melting temperature, viscosity, density, etc.). It is therefore understood that the pouring is an important issue for the person skilled in the art. For example, the pouring conditions influence the scrap rate of the part to be formed.
[0005] In addition, in known methods, it appears that pouring is an obstacle to the formation of bi-material parts. Indeed, to obtain bi-material parts, it would then be necessary to provide two pours and two solidifications in a single furnace; however, it is not possible to pour two alloys into the same crucible.
[0006] One solution could be to change the crucible after the first pour, but changing the crucible is a non-automated operation that requires operator intervention. However, such a change in the furnace in operation represents a considerable risk for the operator. Indeed, the furnace in operation can reach temperatures above 1000 °C. This also represents risks for the furnace itself because opening it during operation causes a significant change in the furnace's thermal properties, which can lead to significant thermal gradients that can cause cracks in the casting stack and leakage of the liquid metal alloy into the furnace.
[0007] It is then understood that pouring is in itself a step which inherently includes significant risks, both from a safety point of view and from the point of view of the quality of the part to be obtained.
[0008] There is therefore a real need for improvement of methods for forming parts using lost wax methods which are free, at least partially, from the inherent disadvantages mentioned above.DISCLOSURE OF THE INVENTION
[0009] The present disclosure relates to a method for forming stack castings, the casting stack comprising a plurality of molds formed by a lost wax method, each mold of the plurality of molds having a vertex, an intermediate portion and a bottom, a bucket capable of receiving liquid metal, a ring connecting the bucket to each vertex of each mold of the plurality of molds, a downcomer connected to the bucket, a plurality of grain selectors each connected to a bottom of a mold of the plurality of molds, the method comprising, inserting a first metal alloy in a solid state into the stack, liquefying the first alloy inserted into the stack, and directed solidification of the first alloy thus liquefied.
[0010] Thus, such a method allows to dispense with pouring. Indeed, in the present method, the metal alloy inserted in a solid state into the casting stack is melted when the casting stack is inserted into a furnace. Consequently, the supply of the metal alloy in the liquid state in the plurality of molds of the casting stack does not require pouring, since the liquid metal alloy is directly obtained by transformation of the solid metal alloy inserted into the casting stack.
[0011] Such a method is therefore safer for the operator. Moreover, handling a metal alloy in the solid state is simpler than handling a metal alloy in the liquid state, so this method is simpler to implement. Moreover, avoiding pouring allows to circumvent the risk of pollution of the liquid metal alloy during said pouring. In addition, this allows to reduce the forces applied by the liquid metal on the casting stack and / or other components.
[0012] In addition, since the liquid metal alloy is formed directly in the casting stack, the risk of handling errors, for example on behalf of the operator, which could lead to accidental pouring of liquid metal alloy into the furnace during the pouring step, disappears.
[0013] In some embodiments, the casting stack further comprises a set of main channels, each channel of the set of main channels connecting the downcomer to a grain selector.
[0014] In this configuration, the casting stack allows the plurality of molds to be filled from their bottom. In particular, in this configuration, a liquid metal alloy can flow from the downcomer to the mold.
[0015] In some embodiments, the first metal alloy is, in the solid state, a single-piece cylindrical ingot.
[0016] In the present application, the expression “cylindrical” is understood in the mathematical sense of the term. A cylinder is defined as the volume obtained by the translation of a closed contour along an axis. For example, the closed contour may be a circle or a square.
[0017] Using a cylindrical ingot makes it easy to calculate the volume of the liquefied metal alloy. Moreover, in this form, the solid metal alloy is easier to insert into the stack.
[0018] In some embodiments, a clearance is provided between the solid metal alloy inserted into the casting stack and the casting stack.
[0019] Thus, this clearance allows for the expansion of the metal alloy under the effect of temperature to be compensated for before it melts. Therefore, this reduces the stresses applied to the casting stack, thereby reducing the risk of leaks.
[0020] In some embodiments, the method further comprises a prior step of assembling the casting stack in which the plurality of molds, the bucket, the ring, the downcomer, and the plurality of grain selectors are assembled together; and in which the first metal alloy in a solid state is inserted into the stack during the prior assembly step.
[0021] In some embodiments, the first metal alloy is inserted into the downcomer.
[0022] In some embodiments, the first metal alloy is inserted into the ring.
[0023] Inserting the metal alloy in a solid state during the assembly step simplifies the integration of the first metal alloy into the stack. Therefore, this represents a time saving for the operator. In particular, the insertion of the first metal alloy into the ring or downcomer is particularly advantageous from this point of view.
[0024] In some embodiments, the casting stack further comprises a plurality of sets of secondary channels, each channel of each set of secondary channels connecting the downcomer and the intermediate portion of a mold, a plurality of plugs delimiting a plurality of casting paths, and wherein a plurality of metal alloys in a solid state are inserted into the plurality of casting paths, the method successively comprising, for each metal alloy of the plurality of metal alloys, the selective liquefaction of the metal alloy followed by the casting of this metal alloy in one of the sets of secondary channels to the plurality of molds, then the solidification, optionally directed solidification, of this liquefied metal alloy.
[0025] In this configuration, it is possible to obtain multi-material parts without resorting to pouring. Furthermore, this method incorporates all the previously mentioned advantages related to the insertion of metal alloys in a solid state into the stack. This configuration is particularly advantageous for forming multi-material turbomachine blades.
[0026] In this disclosure, a “multi-material” part is a part comprising at least two portions made of two different materials. For example, a blade comprising two portions made of two different metal alloys is considered a “multi-material” part.
[0027] Moreover, one of the major challenges when forming multi-material blades is the junction area between the different materials. In particular, controlling the size, position and solidification of the junction area are concerns of interest to the person skilled in the art seeking to manufacture multi-material blades.
[0028] According to this aspect, it is possible to obtain a multi-material part in a single furnace, guaranteeing good properties for the part obtained, in particular at its junction areas between the different materials. Indeed, the insertion of metal alloy in a solid state allows to control more precisely the volume of liquid metal alloy injected into the mold.
[0029] In some embodiments, the casting stack comprises an upper plug placed at the junction between the bucket and the downcomer, and wherein the method comprises: pouring a terminal metal alloy in a liquid state into the bucket, such that the terminal metal alloy flows into each mold of the plurality of molds through the ring, and solidifying the terminal metal alloy.
[0030] Depending on the case, depending on the metal alloy involved and / or the part, pouring is desirable. This configuration therefore allows to obtain a multi-material part by pouring the terminal metal alloy. On the other hand, this configuration represents an alternative and / or a complement for obtaining multi-material parts.
[0031] In some embodiments, the casting stack comprises a container, the container comprising a heating system; and the method further comprising inserting the terminal metal alloy in a solid state into the container, and liquefying the terminal metal alloy by the heating system.
[0032] In some embodiments, the container is attached to the bucket.
[0033] This configuration allows to obtain a multi-material part while avoiding the disadvantages associated with pouring, while retaining the advantages associated with the use of the bucket. Furthermore, according to this embodiment, the casting of the terminal metal alloy is faster than the pouring of this alloy, according to known methods.
[0034] In some embodiments, the container comprises a metal membrane at the junction between the container and the bucket.
[0035] In this configuration, the tightness of the container is improved.
[0036] In some embodiments, the heating system imposes a temperature gradient comprised between 10 °C and 50 °C, preferably 50 °C in the container.
[0037] In some embodiments, the heating system imposes a temperature gradient comprised between 10 °C and 30 °C.
[0038] Thus, this gradient allows to control the melting of the terminal metal alloy, and in particular, to liquefy it gradually. This improves the reliability of the casting of the terminal metal alloy into the plurality of molds in the casting stack.
[0039] In some configurations, a plurality of ceramic cores are provided in the plurality of molds.
[0040] The plurality of ceramic cores allows for a greater diversity of parts. For example, this allows the production of blades called hollow or cooled blades.
[0041] The present disclosure further relates to a turbomachine blade obtained by a method according to one of the preceding embodiments.
[0042] In some configurations, the blade comprises at least two portions made from two different metal alloys, and a junction area between these two portions.
[0043] The above-mentioned features and advantages, as well as others, will become apparent upon reading the following detailed description of exemplary embodiments of the proposed device and method. This detailed description refers to the appended drawings.BRIEF DESCRIPTION OF THE DRAWINGS
[0044] The appended drawings are schematic and are intended primarily to illustrate the principles of the disclosure.
[0045] FIG. 1 schematically shows a casting stack according to a first embodiment of the invention, in which a metal alloy is inserted into the downcomer.
[0046] FIG. 2 schematically shows the casting stack according to the embodiment of FIG. 1, arranged in a furnace, and in which the metal alloy is liquefied.
[0047] FIG. 3 schematically shows the casting stack according to the embodiment of FIG. 1, in which the liquid metal alloy is cast into the plurality of molds.
[0048] FIG. 4 schematically shows the casting stack according to the embodiment of FIG. 1, in which the metal alloy is solidified.
[0049] FIG. 5 schematically shows the casting stack according to the embodiment of FIG. 1, in which the terminal metal alloy is poured into the bucket.
[0050] FIG. 6 schematically shows the casting stack according to the embodiment of FIG. 1, in which the terminal metal alloy is solidified.
[0051] FIG. 7 schematically shows a casting stack according to a second embodiment of the invention, in which a plurality of metal alloys are inserted into the downcomer.
[0052] FIG. 8 schematically shows a casting stack according to a third embodiment of the invention, in which a terminal alloy is inserted into a container.
[0053] FIG. 9 schematically shows a casting stack according to the third embodiment, in which a first metal alloy is liquefied and cast into the plurality of molds.
[0054] FIG. 10 schematically shows a casting stack according to the third embodiment, in which the terminal alloy is liquefied.
[0055] FIG. 11 schematically shows a casting stack according to the third embodiment, in which the terminal alloy is poured into the bucket.
[0056] FIG. 12 schematically shows a fourth embodiment, in which a first metal alloy is stored in solid form in the upper portion of a casting stack.DESCRIPTION OF THE EMBODIMENTS
[0057] In order to make the disclosure more concrete, an example of a device is described in detail below, with reference to the appended drawings. It is recalled that the invention is not limited to this example.
[0058] FIG. 1 schematically shows a casting stack 100 according to a first embodiment of the invention. The casting stack 100 comprises a bucket 101 configured to receive liquid metal, a ring 102, a plurality of molds 103, a grain selector 104, a set of main channels 105, a downcomer 106 connected to the bucket 101, each channel of the set of main channels 105 connecting the downcomer 106 to a grain selector 104.
[0059] The plurality of molds 103 comprises molds formed by a lost wax method, and each mold of the plurality of molds 103 has a vertex, an intermediate portion, and a bottom.
[0060] The ring 102 connects the bucket 101 to each vertex 103a of each mold of the plurality of molds 103, and each grain selector of the plurality of grain selectors 104 is connected to a bottom 103c of a mold of the plurality of molds 103.
[0061] Advantageously, the plurality of molds 103 may comprise a plurality of cores, in order to obtain, for example, hollow blades.
[0062] In the present example, a ceramic upper plug 107 may be provided at the junction between the bucket 101 and the downcomer 106. This plug is impervious to the liquid metal, so that a liquid metal poured into the bucket 101 is forced to flow into the ring 102, then into the plurality of molds 103. When a liquid metal follows such a path, this is referred to as falling liquid metal casting.
[0063] A first metal alloy 10 is inserted into the downcomer 106. The first metal alloy 10 is inserted in the form of a single-piece cylindrical ingot with a circular base. In other examples, the first metal alloy 10 may be inserted into the ring. Furthermore, the first metal alloy 10 may be inserted in the form of shot or in any other solid form making it suitable for insertion into the stack 100.
[0064] In the present example, the downcomer 106 is cylindrical with a circular base. A clearance d is provided between the internal wall of the downcomer 106 and the first metal alloy 10.
[0065] FIG. 2 shows the casting stack 100 of the first embodiment arranged in a Birdgman furnace 50. The furnace 50 comprises a hot area 51 and a cold area 52.
[0066] Initially, the casting stack 100 is placed at the hot area 51 of the furnace 50. The first metal alloy 10 liquefies.
[0067] The volume of liquefied metal alloy 10 is calculated according to the following formula.VS=ρLρS·VL[Math 1]
[0068] With VS the volume of the metal alloy in a solid state, VL the volume of the metal alloy in the liquid state, ρS the density of the metal alloy in a solid state and ρL the density of the metal alloy in the liquid state. Generally, for nickel alloys, the density ratio is of the order of 1.14.
[0069] Knowing the volume of the plurality of molds 103 to be filled, it is possible to deduce the quantity, or volume, of metal alloy 10 to be provided to fill the plurality of molds 103. The inventors have found that it is necessary to provide a volume of solid metal alloy slightly in addition to the volume necessary for filling the plurality of molds 103, to compensate for a residual volume lost during the solidification of the metal alloy, related to the contraction of the metal alloy during said solidification.
[0070] As shown in FIG. 3, the first molten metal alloy 10 follows the set of channels 105 to fill the plurality of molds 103 through their bottom 103c. For example, this filling can be carried out simply by gravity and / or capillarity. When a liquid metal follows such a path, this is called bottom casting of the metal alloy.
[0071] In the present example, the first metal alloy 10 partially fills the plurality of molds 103. However, in other examples, the first metal alloy 10 may completely fill the plurality of molds 10, provided that the adequate volume has been provided.
[0072] As shown in FIG. 4, once the first metal alloy 10 is cast into the plurality of molds 103, the casting stack is transferred (for example by downward gravitational pull of the casting stack or under the action of actuating members such as jacks) to the cold area 52 of the mold so that the first liquid metal alloy 10 is in the cold area 52 of the furnace 50. In this example, only the partially filled portion of the plurality of molds 103 is in the cold area 52 of the furnace 50.
[0073] Thus, the first metal alloy 10 crystallizes in the plurality of molds 103. In the present example, the solidification of the first metal alloy 10 is directed by means of the plurality of grain selectors 104. In other words, the first metal alloy 10 crystallizes in the plurality of molds 103 in a plurality of single-crystal alloys.
[0074] In the present example, after the crystallization of the first metal alloy 10, a terminal metal alloy 20 (FIG. 5), different from the first metal alloy 10, is poured in the liquid state into the bucket 101. Thanks to the upper plug 107, the casting of the terminal metal alloy 20 is falling.
[0075] The terminal metal alloy 20 flows into the plurality of molds 103 and fills the space left empty by the first metal alloy 10. An interface 12 between the first metal alloy 10 and the terminal metal alloy 20 is created. At this interface, diffusion of the terminal metal alloy 20 into the first metal alloy 10 can be observed. In addition, during pouring of the terminal metal alloy 20, partial remelting of the first metal alloy 10 at the interface 12 can be observed.
[0076] Once the terminal metal alloy 20 is poured, as shown in FIG. 6, the entire casting stack 100 is transferred (for example by downward gravitational pull of the casting stack or under the action of actuating members such as jacks) into the cold area 52 of the mold 50. In this way, the terminal metal alloy 20 solidifies. Optionally, the first metal alloy 10 can serve as a seed for directed solidification of the terminal metal alloy 20.
[0077] Once the terminal metal alloy 20 has solidified, a plurality of parts is obtained in the plurality of molds. Different steps of finishing the plurality of parts may be provided.
[0078] FIG. 7 shows a casting stack 100 according to a second embodiment, compatible with the first embodiment. In the example of the second embodiment, the casting stack 100 comprises a plurality of plugs 107′ arranged in the downcomer 106. Furthermore, the casting stack 100 comprises a plurality of sets of secondary channels 105′, each channel of each set of secondary channels 105′ connecting the downcomer 106 and the intermediate portion 103b of a mold of the plurality of molds 103.
[0079] In this way, a plurality of cavities is formed in the downcomer 106 between each of the plurality of plugs 107′. The channels of the plurality of secondary channel sets 105′ are configured to connect each of these cavities to the different molds of the plurality of molds 103. Thus, a plurality of casting paths are formed in the downcomer 106.
[0080] A plurality of metal alloys 10′, different from one another, is inserted into the plurality of cavities formed between the plugs 107. For example, the plugs 107 can be inserted during assembly of the casting stack. Advantageously, the metal alloys of the plurality of metal alloys 10′ each have a different melting temperature. Once the casting stack 100 is placed in the furnace 50, the metal alloys of the plurality of metal alloys 10′ can therefore be selectively liquefied, by appropriate control of the temperature of the hot area 51 of the furnace 50.
[0081] When one alloy of the plurality of alloys 10′ is liquefied, it is cast in the molds of the plurality of molds 103 and solidified in a manner similar to the casting and solidification of the first metal alloy 10. The liquefied first alloy is thus bottom cast.
[0082] Under these circumstances, by selectively liquefying then solidifying the metal alloys of the plurality of metal alloys 10′, a multi-material part is obtained.
[0083] FIG. 8 shows a casting stack 100 according to a third embodiment, compatible with the other embodiments. Apart from the container 200 and the heating system 202 described below, the casting stack 100 according to the third embodiment is in all respects identical to the casting stack 100 of the first embodiment. Furthermore, with the exception of the pouring of the terminal metal alloy 20, the method for obtaining the part for this third embodiment is identical to the first embodiment.
[0084] In the third embodiment, the casting stack 100 comprises a container 200 and a heating system 202 capable of heating the container 200. For example, the heating system 202 may be a heating resistor. The container 200 may be attached to the bucket 101. Alternatively, the container 200 may be attached by other means not shown, and provided above the bucket 101, such that a liquid escaping from the container 200 under the effect of gravity falls into the bucket 101.
[0085] A metal membrane 204, typically made of nickel, may be provided at the junction between the container 200 and the bucket 101.
[0086] In this example, the terminal alloy 20 is inserted into the container 200 in a solid state.
[0087] As shown in FIG. 9, the first metal alloy 10 is liquefied then solidified as described in the first embodiment. Subsequent to this solidification, and as shown in FIG. 10, the heating system 200 liquefies the terminal metal alloy 20. In other examples, the furnace 50 may be capable of liquefying the terminal metal alloy 20.
[0088] As shown in FIG. 11, once the terminal metal alloy 20 is liquefied, the metal membrane 204 is removed and the liquid terminal metal alloy 20 is poured into the bucket 101. The terminal metal alloy 20 is then solidified in a manner similar to the first embodiment.
[0089] The removal of the metal membrane 204 can be carried out by melting the latter. Indeed, once the terminal metal alloy 20 is liquefied, the terminal metal alloy 20 is capable of liquefying the metal membrane 204.
[0090] Alternatively, the container 200 may comprise a bottom instead of the metal membrane 204. Moreover, the bottom comprises an opening which faces the bucket 101. The terminal metal alloy may then have a cylindrical shape, the base of which has a characteristic dimension greater than the characteristic dimension of the opening of the container 200. In these circumstances, when the terminal metal alloy 20 is inserted in a solid state into the container 200, the terminal metal alloy 20 is maintained in a fixed vertical position in the container. However, when the terminal metal alloy 20 is liquefied, the latter is able to be poured into the bucket 101 of the casting stack 100, through the opening of the container 200.
[0091] Optionally, the heating system may be capable of imposing a temperature gradient in the container 200. Under these circumstances, it is possible to partially liquefy the terminal metal alloy 20. This reduces the risk of the appearance of non-liquefied solid grains. Such grains are undesirable because they harm the properties of the part to be formed. These grains are even more undesirable because they can block, for example, the channels of the casting stack 100.
[0092] As shown schematically in FIG. 12, a casting stack 300 similar to the casting stack 100 of FIG. 1 comprises, in addition to the components shown in FIG. 1 and which retain the same references 101, 103, 103a-b, 104, 105, 106 and 107, a storage area for a first metal alloy in solid form which is arranged in the upper portion of the casting stack.
[0093] More particularly, this area includes a plurality of storage containers or cylinders 310 which are arranged respectively above a mold 103 and each connected to the latter (vertex 103a) by a vertical connection 312. The cylinders 310 each contain a first metal alloy 314 in solid form, for example in the form of an ingot (for example: single-piece cylindrical, with a circular base), or in the form of shot or any other solid form. The first alloy has been previously inserted into the stack.
[0094] The ring 302 connects the lower portion of the bucket 101 to the upper portion of the cylinders 310 and the plug 107 is positioned in the upper portion of the downcomer 106 so that the material (second alloy) present in the bucket can be distributed directly into the cylinders without passing through the downcomer.
[0095] In this embodiment, the downcomer 106 is not used. The method described here can therefore be used in a casting stack configuration not comprising a downcomer.
[0096] In this embodiment, the casting stack 300 is introduced into the hot area 51 of a furnace 50 as in the mode illustrated in FIG. 2 and the first alloy 314 is liquefied inside the cylinders 310, which allows it to flow directly from each cylinder 310 into the mold located below (drop filling method) through the connection 312. The configuration of the casting stack 300 is advantageous compared to that of the casting stack 100 of FIG. 1 insofar as the storage area of the first metal alloy 314 is arranged as close as possible to the heating elements and / or radiant walls of the furnace (on the periphery of the casting stack and not in the center thereof as in the downcomer 106). The storage area of the first metal alloy 314 is therefore not masked by a component of the casting stack which would be arranged between said component and the heating elements and / or radiant walls of the furnace and is therefore directly exposed to the heating radiation. This results in greater operating efficiency.
[0097] As in FIG. 4, the casting stack 300 is then lowered vertically partly into the cold area 52 of the furnace 50 in order to solidify the first metal alloy 314.
[0098] As in FIG. 5, after the crystallization of the first metal alloy, a terminal metal alloy (second alloy), different from the first metal alloy, is poured in the liquid state into the bucket 101. Thanks to the upper plug 107, the casting of the terminal metal alloy is falling and is distributed in the ring 302 up to the cylinders 310 in which the terminal metal alloy flows, to reach, via the connections 312, the plurality of molds 103 and fill in the latter the space left empty by the first metal alloy 314. The remainder of the description of the first mode applies here and will not be repeated.
[0099] Although the present invention has been described with reference to specific exemplary embodiments, it is obvious that modifications and changes may be made to these examples without departing from the general scope of the invention as defined by the claims. In particular, individual features of the various illustrated / mentioned embodiments may be combined in additional embodiments.
[0100] Therefore, the description and drawings should be considered in an illustrative rather than restrictive sense.
[0101] It is also obvious that all the characteristics described with reference to a method are transposable, alone or in combination, to a device, and conversely, all the characteristics described with reference to a device are transposable, alone or in combination, to a method.
Claims
1. A method for forming stack castings, the casting stack comprising:a plurality of molds formed by a lost wax method, each mold of the plurality of molds having a vertex, an intermediate portion and a bottom,a bucket capable of receiving liquid metal,a ring connecting the bucket to each vertex of each mold of the plurality of molds,a downcomer connected to the bucket,a plurality of grain selectors each connected to a bottom of a mold of the plurality of molds,the method comprising,inserting a first metal alloy in a solid state into the stack,liquefying the first alloy inserted into the stack,directed solidification of the first alloy thus liquefied.
2. The method according to claim 1, wherein the casting stack further comprises a set of main channels, each channel of the set of main channels connecting the downcomer to a grain selector.
3. The method according to claim 1, wherein the first metal alloy is, in the solid state, a single-piece cylindrical ingot.
4. The method according to claim 1, further comprising a prior step of assembling the casting stack in which the plurality of molds, the bucket, the ring, the downcomer and the plurality of grain selectors are assembled together; andin which the first metal alloy in a solid state is inserted into the casting stack during the prior assembly step.
5. The method according to claim 1, wherein the casting stack further comprises:a plurality of sets of secondary channels, each channel of each set of secondary channels connecting the downcomer and the intermediate portion of a mold,a plurality of plugs delimiting a plurality of casting paths, andwherein a plurality of metal alloys in a solid state are inserted into the plurality of casting paths,the method successively comprising, for each metal alloy of the plurality of metal alloys, the selective liquefaction of the metal alloy followed by the casting of this metal alloy in one of the sets of secondary channels to the plurality of molds, then the solidification of this liquefied metal alloy.
6. The method according to claim 1, wherein the casting stack comprises an upper plug placed at the junction between the bucket and the downcomer, andwherein the method comprises:pouring a terminal metal alloy in a liquid state into the bucket, such that the terminal metal alloy flows into each mold of the plurality of molds through the ring, andsolidifying the terminal metal alloy.
7. The method according to claim 6, wherein the casting stack comprises a container, the container comprising a heating system; andthe method further comprisinginserting the terminal metal alloy in a solid state into the container, andliquefying the terminal metal alloy by the heating system.
8. The method according to claim 7, wherein the container comprises a metal membrane at the junction between the container and the bucket.
9. The method according to claim 7, wherein the heating system imposes a temperature gradient comprised between 10 °C and 50 °C in the container.
10. The method according to claim 1, wherein a plurality of ceramic cores are provided in the plurality of molds.
11. A turbomachine blade obtained by a method according claim 1.
12. The blade according to claim 11, comprising at least two portions made from two different metal alloys, and a junction area between these two portions.