Method for manufacturing a stainless steel

By thermochemically treating nickel hyperaccumulator plants to produce nickel-rich ash or biochar and using it to manufacture stainless steel, the method addresses the high costs and environmental impact of traditional nickel ore-based stainless steel production, achieving cost-effective and eco-friendly steel manufacturing.

US20260366092A1Pending Publication Date: 2026-11-19APERAM +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
US19/155145
Authority / Receiving Office
US · United States
Patent Type
Applications(United States)
Current Assignee / Owner
Filing Date
2023-02-09
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

The existing methods for manufacturing stainless steel from nickel-rich ores are costly and environmentally detrimental due to high nickel ore prices and significant environmental impact, including soil and hydrosphere destruction, and CO2 emissions.

Method used

A method involving the thermochemical treatment of nickel hyperaccumulator plants to produce nickel-rich ash or biochar, followed by briquetting and pyrometallurgical processing to create a ferroalloy with a high nickel content, which is then used to produce stainless steel, minimizing the use of nickel-rich ores and reducing environmental impact.

Benefits of technology

This method reduces production costs and environmental harm by utilizing bio-sourced nickel, decreasing soil degradation, hydrosphere pollution, and CO2 emissions, while maintaining high nickel yield and steel quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure US20260366092A1-D00000_ABST
    Figure US20260366092A1-D00000_ABST
Patent Text Reader

Abstract

The invention relates to a method for manufacturing a stainless steel:a. manufacturing (10) a ferroalloy, comprising:providing (12) plant material having a nickel content of 0.5% or more by dry weight;thermochemically treating (14) the plant material in order to obtain nickel-rich ash having a nickel content of 10% or more by weight or nickel-rich biochar having a nickel content of 2% or more by weight;manufacturing (16) briquettes from the nickel-rich ash or from a homogenate of the nickel-rich biochar, comprising adjusting the phosphorus content such that the briquettes have a ratio of the nickel content by weight to the phosphorus content by weight of 40 or more; andmanufacturing (18) a ferroalloy from the briquettes by pyrometallurgy, the ferroalloy having a nickel content of between 4% and 50% by weight; andb. preparing (20) a stainless steel from the ferroalloy.
Need to check novelty before this filing date? Find Prior Art

Description

The present invention relates to a method for manufacturing a stainless steel from a ferroalloy containing between 4% and 50% by weight of nickel.Ferroalloys containing nickel at concentrations greater than or equal to 4% by weight are usually obtained by pyrometallurgy from nickel-rich ores, such as laterites.This method, however, does not provide complete satisfaction. Indeed, it is relatively costly, particularly due to the relatively high price of nickel-rich ore. Furthermore, the extraction of nickel-rich ore has a significant environmental impact, particularly in terms of deep soil and hydrosphere destruction, as well as local fauna and flora. Additionally, nickel extraction leads to direct CO2 emissions between 10 and 100 tons of CO2 per ton of nickel equivalent in the production of nickel pig iron.An objective of the invention is to provide a method for manufacturing a stainless steel with reduced environmental impact and cost.To this end, the invention relates to a method for manufacturing a stainless steel, comprising the following successive steps:a. manufacturing a ferroalloy, comprising:providing plant material, said plant material having a nickel content greater than or equal to 0.5% by dry mass;

[0008] thermochemically treating the plant material in a thermochemical treatment unit to obtain nickel-rich ash with a nickel content greater than or equal to 10% by weight or nickel-rich biochar with a nickel content greater than or equal to 2% by weight;

[0009] manufacturing briquettes from the nickel-rich ash or a homogenate of the nickel-rich biochar, comprising adjusting the phosphorus content such that the briquettes have a ratio of the nickel content by weight to the phosphorus content by weight greater than or equal to 40; and

[0010] manufacturing a ferroalloy by pyrometallurgy from the briquettes, the ferroalloy having a nickel content between 4% and 50% by weight; and

[0011] b. preparing a stainless steel from the ferroalloy.

[0012] The manufacturing method according to the invention may also comprise one or more of the following features, taken alone or in any technically possible combination:

[0013] the thermochemical treatment is combustion in the presence of oxygen at a temperature between 550 °C and 1200 °C to obtain nickel-rich ash;

[0014] the combustion is carried out between 800 °C and 1100 °C;

[0015] adjusting the phosphorus content comprises:

[0016] a. mixing nickel-rich ash from plants associated with different combinations of species, geographical origins, and harvest years to obtain a predefined ratio of nickel content by weight to phosphorus content by weight, for example, greater than or equal to 40, in the mixture; and / or

[0017] b. washing the nickel-rich ash to reduce its phosphorus content; and / or

[0018] c. mixing the nickel-rich ash with other nickel-containing materials to obtain in the mixture a value of the ratio of nickel content by weight to phosphorus content by weight greater than the value of the nickel content by weight to phosphorus content by weight in the nickel-rich ash;

[0019] the washing of the ash is carried out in an acidic solution for a duration between 5 minutes and 10 minutes at a temperature between 5 °C and 50 °C;

[0020] the acidic solution is an aqueous solution containing 0.1 to 4 mol / L of protons;

[0021] the ratio of nickel content by weight to phosphorus content by weight of the nickel-rich ash or the homogenate of nickel-rich biochar is less than 40;

[0022] the manufacturing of briquettes comprises:

[0023] a. manufacturing a mixture comprising the nickel-rich ash, as well as a binder, a source of reducing agent, a flux, and optionally additional materials providing alloying elements for the ferroalloy; and

[0024] b. compressing this mixture to obtain the briquettes;

[0025] the additional materials come at least in part from sludge or dust from the metallurgical industry;

[0026] the thermochemical treatment is pyrolysis to obtain nickel-rich biochar, the method further comprising a step of grinding the biochar to obtain a homogenate of biochar;

[0027] adjusting the phosphorus content comprises:

[0028] mixing nickel-rich biochars from plants characterized by different combinations of species, geographical origins, and harvest years to obtain a predefined ratio of nickel content by weight to phosphorus content by weight, for example, greater than or equal to 40, in the mixture; and / or

[0029] mixing the nickel-rich biochar with other nickel-containing materials to obtain in the mixture a value of the ratio of nickel content by weight to phosphorus content by weight greater than the value of the nickel content by weight to phosphorus content by weight in the nickel-rich biochar;

[0030] the manufacturing of briquettes comprises:

[0031] manufacturing a mixture comprising the homogenate of nickel-rich biochar, as well as a binder, a flux, and additional materials providing alloying elements for the ferroalloy; and

[0032] compressing this mixture to obtain the briquettes;

[0033] the additional materials come at least in part from sludge or dust from the metallurgical industry;

[0034] the plant material is provided in the form of a homogenate of plants, particularly in the form of granules comprising the homogenate of plants;

[0035] the step of providing plant material comprises:

[0036] providing dried plants;

[0037] grinding the dried plants to obtain a homogenate of plants; and optionally

[0038] compressing this homogenate of plants to obtain granules;

[0039] the method further comprises, during the compression step to form the granules, heating the homogenate of plants to a temperature between 60 °C and 80 °C;

[0040] the method further comprises, during the compression step to form the granules, adding an adjuvant intended to facilitate the agglomeration of the homogenate of plants, the adjuvant being, preferably, water;

[0041] the plant material is obtained from nickel hyperaccumulator plants, for example, chosen from the following species:

[0042] Odontarrhena chalcidica (syn=Alyssum murale)

[0043] Bornmuellera emarginata (syn=Leptoplax emarginata)

[0044] Bornmuellera tymphaea

[0045] Berkheya coddii

[0046] Blepharidium guatemalense

[0047] Phyllanthus rufuschaneyi

[0048] Rinorea aff. bengalensis.

[0049] adjusting the phosphorus content is carried out such that the briquettes have a ratio of nickel content by weight to phosphorus content by weight greater than or equal to 80;

[0050] the manufacturing of the ferroalloy by pyrometallurgy from the briquettes comprises:

[0051] introducing the briquettes into a furnace;

[0052] melting the briquettes in the furnace to obtain a liquid ferroalloy, the ferroalloy comprising between 4% and 50% by weight of nickel, and

[0053] casting the ferroalloy in the form of a semi-product, for example, in the form of ingots or granules;

[0054] the manufacturing of stainless steel from the ferroalloy comprises:

[0055] providing a mixture of ferroalloy and scrap, the scrap comprising notably stainless steel scrap;

[0056] melting this mixture in an electric furnace, particularly an electric arc furnace, to obtain a liquid steel; and

[0057] refining this liquid steel to obtain stainless steel.

[0058] The invention will be better understood by reading the following description, given solely by way of example, and made with reference to the attached figure, which is a schematic view of the method for manufacturing stainless steel according to the invention.

[0059] The method for manufacturing a stainless steel according to the invention comprises the following successive steps:

[0060] manufacturing 10 a ferroalloy, comprising:

[0061] providing 12 plant material;

[0062] thermochemically treating 14 the plant material to obtain nickel-rich ash or nickel-rich biochar;

[0063] manufacturing 16 briquettes from the nickel-rich ash or a homogenate of nickel-rich biochar;

[0064] manufacturing 18 a ferroalloy by pyrometallurgy from the briquettes; and

[0065] preparing 20 a stainless steel from the ferroalloy.

[0066] More particularly, the plant material provided in step 12 has a nickel content greater than or equal to 0.5% by dry mass, and particularly greater than or equal to 1% by dry mass.

[0067] The plant material provided in step 12 comprises, for example, a phosphorus content between 1000 to 4000 mg / kg of plant material.

[0068] This plant material is obtained from nickel hyperaccumulator plants.

[0069] By “nickel hyperaccumulator plant,” we mean a plant capable of storing in its aerial parts a nickel concentration greater than or equal to 1000 μg / g of dry matter. The nickel stored in the aerial parts of the plant comes from the soil wherein the plant is grown.

[0070] For example, depending on the geographical area, nickel hyperaccumulator plants are chosen from the following species:

[0071] Odontarrhena chalcidica (syn=Alyssum murale)

[0072] Bornmuellera emarginata (syn=Leptoplax emarginata)

[0073] Bornmuellera tymphaea

[0074] Berkheya coddii

[0075] Blepharidium guatemalense

[0076] Phyllanthus rufuschaneyi

[0077] Rinorea aff. bengalensis.

[0078] The step of providing 12 plant material preferably comprises a step of providing dried plants.

[0079] Preferably, the plants are dried to have a moisture content less than or equal to 20%. Indeed, a moisture content greater than 20% may lead to degradation, particularly mold development, of the plants during their storage before grinding.

[0080] The drying of the plants is advantageously carried out in the open air, notably in the field after harvesting the plants.

[0081] Alternatively, and notably in cases where the plants are grown in regions where the air humidity is high so that open-air drying results in a plant moisture content greater than 20%, the drying comprises a step of heating the plants to a temperature and for a duration adapted to obtain a moisture content less than or equal to 20%, and preferably between 5% and 20%.

[0082] The dried plants also preferably have a moisture content greater than or equal to 5%. Indeed, such a moisture content is favorable for the agglomeration of dried plants in the form of granules. A moisture content greater than or equal to 5% is notably obtained by adjusting the drying time of the plants in the open air and / or the temperature and duration of heating in an adapted manner.

[0083] The dried plants thus preferably have a moisture content between 5% and 20%.

[0084] According to one example, the moisture content of the dried plants is approximately equal to 15%.

[0085] According to one embodiment, step 12 of providing plant material comprises:

[0086] providing dried plants as described above; and

[0087] grinding the dried plants to obtain a homogenate of plants.

[0088] More particularly, during step 12 of providing plant material, the plant material is provided in the form of granules comprising this homogenate of plants. According to this embodiment, step 12 of providing plant material comprises a step of manufacturing granules from this homogenate of plants.

[0089] The step of manufacturing granules optionally comprises compressing the homogenate of plants to obtain the granules.

[0090] In this case, the step of grinding the dried plants to obtain a homogenate of plants is carried out in a manner to obtain a homogenate of plants with a particle size suitable for manufacturing granules by compression. This particle size is notably between 3 mm and 5 mm. However, other particle sizes are possible depending on the desired dimensions of the granules and the compaction ability of the plants used.

[0091] The step of compressing the homogenate of plants to form the granules is notably carried out by extrusion in a die.

[0092] The length of the granules is determined by the compression device used, particularly the die. The maximum length of the granules is chosen to prevent the granules from breaking during storage and / or transport. For example, the granules have a length between 20 mm and 40 mm, and for example, approximately equal to 27 mm.

[0093] The step of compressing the homogenate of plants to form the granules optionally comprises heating the homogenate of plants to a temperature between 60 °C and 80 °C. This heating step is preferably carried out simultaneously with the compression. It facilitates the agglomeration of the homogenate of plants in the form of granules.

[0094] Optionally, the compression step also comprises adding an adjuvant intended to facilitate the agglomeration of the homogenate of plants. This adjuvant is preferably water. The amount of adjuvant added during this step is chosen based on the initial moisture content of the dried plants to achieve sufficient agglomeration of the homogenate of plants.

[0095] According to a first embodiment of the method, the thermochemical treatment step 14 of the plant material is a combustion step to obtain nickel-rich ash. Depending on the composition of the plant material, the nickel-rich ash may contain, in addition to nickel, other elements of interest in the context of stainless steel manufacturing, such as magnesium, silicon, iron, or calcium.

[0096] The combustion step is carried out in a combustion unit in the presence of oxygen at a temperature between 550 °C and 1200 °C. More particularly, the combustion temperature is between 800 °C and 1100 °C, and is notably approximately equal to 900 °C.

[0097] The combustion is carried out in the presence of excess oxygen to achieve complete combustion of the plant material. For example, oxygen is supplied through an air inlet provided in the combustion unit.

[0098] The combustion unit is, for example, a furnace or a biomass boiler.

[0099] At the end of this combustion step, nickel-rich ash is obtained with a nickel content greater than or equal to 10% by weight, and for example, between 10% by weight and 40% by weight.

[0100] In the ash, nickel is in the form of nickel oxide NiOx.

[0101] These ashes also have a phosphorus content greater than or equal to 0.5% by weight, and notably between 0.5% by weight and 5% by weight. In the ash, phosphorus is typically present in the form of apatite Ca5(PO4)3(OH) and related forms.

[0102] In the ash, the ratio of nickel content by weight to phosphorus content by weight is, for example, less than 40.

[0103] The ash may also contain other chemical elements, notably calcium, for example, at a content between 10% by weight and 40% by weight and potassium, for example, at a content between 2% by weight and 15% by weight. Calcium and potassium are typically present in the ash in the form of oxides, particularly carbonates, hydroxyapatite Ca5(PO4)3(OH), potassium sulfate (K2SO4), or potassium chloride (KCl).

[0104] The precise composition of the ash depends notably on the nature of the plant material, the soil wherein it was grown, the amendments applied to the soil (fertilizers, manure, composts, etc.), the combustion temperature used, and the climatic conditions.

[0105] The step of manufacturing 16 briquettes from nickel-rich ash comprises:

[0106] manufacturing a mixture comprising the nickel-rich ash, as well as a binder, a source of reducing agent, a flux, and optionally additional materials providing alloying elements for the ferroalloy; and

[0107] compressing this mixture to obtain the briquettes.

[0108] The binder used is, for example, molasses. Its function is to bind the various constituents of the relatively dry mixture together to allow the manufacture of briquettes.

[0109] The reducing agent comprises, in particular, carbon, aluminum, and / or silicon. It allows, during the subsequent treatment of the briquettes in the combustion unit, the reduction of the oxides contained in the briquettes, notably the reduction of nickel oxide to metallic nickel. In the case where carbon is used as a reducing agent, the carbon is, for example, provided in the form of anthracite or biochar.

[0110] The flux is, for example, lime. The flux allows the removal of certain undesirable impurities from the alloy during the subsequent treatment of the briquettes in the furnace. In particular, the flux fuses with these impurities to form slags that separate from the alloy and can then be removed.

[0111] The mixture optionally contains additional materials, different from the ash, allowing the addition of additional alloying elements. These additional materials comprise, in particular, materials containing nickel, iron, molybdenum, calcium, and / or chromium. These additional materials are, for example, provided in the form of sludge or dust from the metallurgical industry and, optionally, metals, for example, nickel or molybdenum, added as dopants. In the sludge and dust from the metallurgical industry, the elements of interest, such as nickel, iron, molybdenum, calcium, and / or chromium, are usually present in the form of oxides.

[0112] Optionally, the sub-step of manufacturing the mixture in step 16 of manufacturing briquettes comprises:

[0113] manufacturing a first mixture comprising the nickel-rich ash, the reducing agent, and optionally the additional materials providing alloying elements for the ferroalloy;

[0114] drying this first mixture; and

[0115] mixing this first mixture with the binder and the flux.

[0116] According to the invention, step 16 of manufacturing briquettes comprises adjusting the phosphorus content such that the briquettes have a ratio of nickel content by weight to phosphorus content by weight greater than or equal to 40. Preferably, the adjustment of the phosphorus content is carried out such that the briquettes have a ratio of nickel content by weight to phosphorus content by weight greater than or equal to 80.

[0117] Such an adjustment is necessary in the context of the method for manufacturing a stainless steel according to the invention. Indeed, the plant material used in the context of the invention typically comprises a phosphorus content of about 1000 to 4000 mg / kg of plant material. This phosphorus comes notably from the fertilizers used for the growth of the plants forming the plant material. However, phosphorus is undesirable in the context of stainless steel manufacturing, as it deteriorates its properties. Therefore, according to European standards, the phosphorus content of stainless steels must typically be less than 0.045%.

[0118] In the context of the present invention, briquettes are considered suitable for stainless steel manufacturing if they have a ratio of nickel content by weight to phosphorus content by weight greater than or equal to 40.

[0119] The higher the ratio of nickel content by weight to phosphorus content by weight, the more nickel from the combustion of plant material as described below can be used in the context of the stainless steel manufacturing method. Therefore, to maximize the use of bio-sourced nickel, the ratio of nickel content by weight to phosphorus content by weight is preferably greater than or equal to 80.

[0120] More particularly, the step of adjusting the phosphorus content comprises:

[0121] (a) mixing nickel-rich ash from plants characterized by different combinations of species, geographical origins, and harvest years to obtain a predefined ratio of nickel content by weight to phosphorus content by weight, for example, greater than or equal to 40, in the mixture;

[0122] (b) washing the nickel-rich ash from the combustion step to reduce its phosphorus content; and / or

[0123] (c) mixing the nickel-rich ash from the combustion step with other nickel-containing materials to obtain in the mixture a value of the ratio of nickel content by weight to phosphorus content by weight greater than the value of the nickel content by weight to phosphorus content by weight in the ash.

[0124] The composition of the plant, and in particular, the nickel and / or phosphorus content of the plant depends on the species of the plant, its geographical origin, as well as its harvest year, and notably the climatic conditions associated with it. Therefore, it is possible to adjust the ratio of nickel content to phosphorus content in the ash by mixing ash obtained from plants with different combinations of species, geographical origins, and harvest years.

[0125] Each type of ash used to make the ash mixture according to alternative (a) is, in particular, obtained by implementing the thermochemical treatment step 14 as described above with plant material obtained from plants characterized by a particular combination of species, geographical origins, and harvest years.

[0126] The mixing of ash from plants characterized by different combinations of species, geographical origins, and harvest years, the washing of the ash, and the mixing of the ash with other nickel-containing materials are, in the context of the invention, used either alternatively or in combination, depending on the phosphorus content of the ash, as well as the quantity of ash available.

[0127] For example, the adjustment of the phosphorus content is carried out only by washing the ash and / or by mixing ash from plants corresponding to different combinations of species, geographical origins, and harvest years in a case where the amount of nickel contained in the ash is sufficient on its own to ensure the desired nickel content in the ferroalloy subsequently manufactured by pyrometallurgy. In this case, the use of bio-sourced ash in the context of the stainless steel manufacturing method is maximized.

[0128] Preferably, the adjustment of the phosphorus content is carried out only by washing the ash.

[0129] Alternatively, the adjustment of the phosphorus content is carried out by mixing nickel-rich ash with other nickel-containing materials, for example, in the case where the amount of nickel contained in the ash is insufficient on its own to ensure the desired nickel content in the ferroalloy subsequently manufactured by pyrometallurgy.

[0130] The washing of the ash is carried out before the step of manufacturing the mixture with the binder, the source of reducing agent, the flux, and the additional materials providing alloying elements described above.

[0131] For example, the washing of the ash comprises:

[0132] contacting the ash with an acidic solution for a sufficient duration to reduce the phosphorus content of the ash;

[0133] filtering this mixture to separate the solid fraction, namely the washed ash, from the liquid fraction, namely an acidic aqueous solution also containing the chemical elements extracted from the ash, particularly phosphorus.

[0134] More particularly, the ash is contacted with the acidic solution for a duration between 5 minutes and 10 minutes at a temperature between 5 °C and 50 °C, and more particularly at a temperature between 15 °C and 25 °C, for example, approximately equal to 20 °C.

[0135] Preferably, the acidic solution is, in particular, an aqueous solution containing 0.1 mol / L to 4 mol / L of protons, for example, an aqueous solution of sulfuric acid, hydrochloric acid, nitric acid, or their mixtures.

[0136] For example, the acidic solution is an aqueous solution of sulfuric acid with a concentration between 0.05 mol / L and 2 mol / L.

[0137] In addition to phosphorus, the liquid fraction obtained after filtration may also contain other chemical elements extracted from the ash, particularly potassium and calcium.

[0138] Optionally, at least some of the chemical elements extracted from the ash, particularly phosphorus and / or potassium, are then extracted from the liquid fraction by any suitable method. These elements are, for example, reusable as fertilizers. The extraction of these chemical elements is carried out by any suitable method, notably by decantation after concentration.

[0139] According to a variant, the washing of the ash comprises, before contacting the ash with the solution described above, a preliminary washing of the ash with water. This preliminary water washing step allows the extraction of at least part of the potassium contained in the ash.

[0140] Optionally, after extracting the chemical elements extracted from the ash from the liquid fraction, the acidic aqueous solution is reused in the context of washing the ash.

[0141] At the end of the washing step, ash is obtained with a phosphorus content reduced compared to their its content before washing by a reduction factor of about 10.

[0142] The washing step allows the solubilization of the phosphorus present in the ash, without solubilizing the nickel.

[0143] The washed ash is then mixed with the binder, the reducing agent, the flux, and optionally the additional materials providing alloying elements necessary for the production of the ferroalloy during the mixing step described above.

[0144] The manufacturing of the ferroalloy by pyrometallurgy from the briquettes comprises:

[0145] introducing the briquettes into a furnace; and

[0146] melting the briquettes in the furnace to obtain a liquid ferroalloy, the ferroalloy comprising between 4% and 50% by weight of nickel.

[0147] The sub-step of introducing the briquettes optionally comprises introducing scrap. The scrap is notably useful during the startup phase of the electric arc furnace, as explained later. For example, during this sub-step, a quantity of scrap between 10 tons and 20 tons is introduced.

[0148] The melting of the briquettes in the furnace is accompanied by a reduction of the metal oxides contained in the briquettes.

[0149] The melting step is particularly carried out in an electric arc furnace. In this case, the sub-step of introducing the briquettes also comprises introducing scrap. This scrap is melted during the startup phase of the electric arc furnace and forms a molten bed at the bottom of the electric arc furnace, also called a “bath bottom.” This “bath bottom” is necessary to initiate melting in the electric arc furnace.

[0150] The manufacturing of the ferroalloy by pyrometallurgy also comprises casting the liquid ferroalloy into semi-products, particularly casting the liquid ferroalloy into ingots in suitable molds or granules by granulation.

[0151] By granulation, we mean casting the liquid ferroalloy into a water jet.

[0152] In the case where the semi-products are ingots, these ingots are optionally mechanically divided into ferroalloy blocks.

[0153] The ferroalloy thus obtained is an iron-based alloy, comprising between 4% and 50% nickel and, optionally, depending on the composition of the raw materials used, molybdenum and / or chromium. For example, the ferroalloy contains between 0% by weight and 10% by weight of molybdenum and between 10% by weight and 20% by weight of chromium. The nickel content of the ferroalloy is essentially defined by the nickel content of the briquettes, with the nickel yield of the method being greater than 95%.

[0154] Finally, the step of manufacturing a stainless steel from the ferroalloy comprises:

[0155] providing a mixture of the ferroalloy with scrap, the scrap comprising notably stainless steel scrap;

[0156] melting this mixture in an electric furnace, particularly an electric arc furnace, to obtain a liquid steel; and

[0157] refining this liquid steel to obtain stainless steel.

[0158] The refining step notably comprises a first refining step carried out in a converter, particularly an AOD (“Argon Oxygen Decarburization”) converter, followed by a second refining step, carried out in a ladle.

[0159] In particular, the refining steps allow the purification of the liquid steel and the adjustment of its composition to the desired composition for stainless steel.

[0160] At the end of the refining step, the stainless steel is cast into semi-products, notably slabs or blooms.

[0161] The step of manufacturing stainless steel is known in itself and is therefore not described in more detail.

[0162] The method for manufacturing stainless steel according to the invention is advantageous. Indeed, by means of the invention of using nickel hyperaccumulator plants as a source of nickel for the manufacture of the ferroalloy, it allows the use of nickel from nickel-rich ores to be avoided, or at least reduced, and thus not only reduces the costs associated with the manufacture of stainless steels but also improves the environmental impact related to the manufacture of these steels. Indeed, it enables reduction of soil, subsoil, and hydrosphere degradation associated with ore extraction, participation in soil depollution through the use of nickel hyperaccumulator plants, and reduction of CO2 emissions associated with the manufacture of the ferroalloy.

[0163] The method according to a second embodiment differs from the method according to the first embodiment only by the nature of the thermochemical treatment step 14 of the plant material, as well as by the step of manufacturing 16 the briquettes.

[0164] In the second embodiment, the thermochemical treatment 14 is pyrolysis, not combustion. Pyrolysis allows nickel-rich biochar to be obtained from the plant material, rather than ash as described in the context of the first embodiment.

[0165] Pyrolysis is carried out in a pyrolysis unit.

[0166] At the end of the pyrolysis step, nickel-rich biochar is obtained with a nickel content greater than or equal to 2% by weight, and for example, greater than or equal to 4% by weight.

[0167] The phosphorus content of the biochar is greater than or equal to 0.5% by weight, and notably between 0.5% and 5%.

[0168] In the biochar, the ratio of nickel content by weight to phosphorus content by weight is, for example, less than 40.

[0169] By biochar, we mean a solid material obtained by pyrolysis of plant material.

[0170] The precise composition of the biochar depends notably on the nature of the plant material, the soil wherein it was grown, the amendments applied to the soil (fertilizers, manure, composts, etc.), the combustion temperature used, and the climatic conditions.

[0171] The other method steps described in the context of the method according to the first embodiment are identical in the context of the method according to the second embodiment, except for the differences described below.

[0172] The steps implemented on the ash obtained at the end of the thermochemical treatment step 14 by combustion in the first embodiment are, in the second embodiment, implemented on a homogenate of nickel-rich biochar obtained at the end of the thermochemical treatment step by pyrolysis.

[0173] In the second embodiment, the method comprises a step of grinding the biochar implemented between the thermochemical treatment step 14 and the step of manufacturing the briquettes 16 to obtain the homogenate of nickel-rich biochar.

[0174] In the context of the method according to the second embodiment, step 16 of manufacturing briquettes from the homogenate of nickel-rich biochar thus comprises:

[0175] manufacturing a mixture comprising the homogenate of nickel-rich biochar, as well as a binder, a flux, and additional materials providing alloying elements for the ferroalloy; and

[0176] compressing this mixture to obtain the briquettes.

[0177] Indeed, in the context of the method according to the second embodiment, the nickel-rich biochar, which contains carbon, plays the role of a reducing agent for the pyrometallurgy step. It is therefore not necessary to add an additional reducing agent to the mixture, as described in the context of the first embodiment.

[0178] The binder and the flux have the same characteristics as described above concerning the first embodiment.

[0179] The additional materials, different from the biochar, allow the addition of additional alloying elements. These additional materials comprise, in particular, materials containing nickel, iron, molybdenum, calcium, and / or chromium. These additional materials are, for example, provided in the form of sludge or dust from the metallurgical industry and, optionally, metals, for example, nickel or molybdenum, added as dopants. In the sludge and dust from the metallurgical industry, the elements of interest, such as nickel, iron, molybdenum, calcium, and / or chromium, are usually present in the form of oxides.

[0180] In this embodiment, the sub-step of manufacturing the mixture in step 16 of manufacturing briquettes optionally comprises:

[0181] manufacturing a first mixture comprising the nickel-rich biochar and optionally the additional materials providing alloying elements for the ferroalloy;

[0182] drying this first mixture; and

[0183] mixing this first mixture with the binder and the flux.

[0184] In the context of the method according to the second embodiment, adjusting the phosphorus content comprises:

[0185] (a) mixing nickel-rich biochars from plants characterized by different combinations of species, geographical origins, and harvest years to obtain a ratio of nickel content by weight to phosphorus content by weight greater than or equal to 40; and / or

[0186] (b) mixing the nickel-rich biochar obtained by the pyrolysis step with other nickel-containing materials to obtain in the mixture a value of the ratio of nickel content by weight to phosphorus content by weight greater than the value of the nickel content by weight to phosphorus content by weight in the ash.

[0187] Each type of biochar used to make the biochar mixture according to alternative (a) is, in particular, obtained by implementing the thermochemical treatment step 14 as described above with plant material obtained from plants characterized by a particular combination of species, geographical origins, and harvest years.

[0188] As indicated above, the steps of providing 12 plant material, manufacturing 18 the ferroalloy from the briquettes, and manufacturing stainless steel from the ferroalloy are identical in the first and second embodiments.

[0189] The manufacturing method according to the second embodiment has the same advantages as the manufacturing method according to the first embodiment.

[0190] Furthermore, since the biochar contains carbon, the method according to the second embodiment has the additional advantage of providing, in addition to nickel, at least part of the reducing agent necessary for the step of manufacturing the ferroalloy by pyrometallurgy.

Claims

1. A method for manufacturing a stainless steel, comprising the following successive steps:a. manufacturing (10) a ferroalloy, comprising:providing (12) plant material, said plant material having a nickel content greater than or equal to 0.5% by dry mass;thermochemically treating (14) the plant material in a thermochemical treatment unit to obtain nickel-rich ash with a nickel content greater than or equal to 10% by weight or nickel-rich biochar with a nickel content greater than or equal to 2% by weight;manufacturing (16) briquettes from the nickel-rich ash or a homogenate of nickel-rich biochar, comprising adjusting the phosphorus content such that the briquettes have a ratio of nickel content by weight to phosphorus content by weight greater than or equal to 40; andmanufacturing (18) a ferroalloy by pyrometallurgy from the briquettes, the ferroalloy having a nickel content between 4% and 50% by weight; andb. preparing (20) a stainless steel from the ferroalloy.

2. The manufacturing method according to claim 1, wherein the thermochemical treatment (14) is combustion in the presence of oxygen at a temperature between 550 °C and 1200 °C to obtain ash.

3. The manufacturing method according to claim 2, wherein the combustion is carried out between 800 °C and 1100 °C.

4. The manufacturing method according to claim 2, wherein adjusting the phosphorus content comprises:a. mixing nickel-rich ash from plants associated with different combinations of species, geographical origins, and harvest years to obtain a predefined ratio of nickel content by weight to phosphorus content by weight in the mixture;b. washing the nickel-rich ash to reduce its phosphorus content; and / orc. mixing the nickel-rich ash with other nickel-containing materials to obtain in the mixture a value of the ratio of nickel content by weight to phosphorus content by weight greater than the value of the nickel content by weight to phosphorus content by weight in the nickel-rich ash5. The manufacturing method according to claim 4, wherein the washing of the ash is carried out in an acidic solution for a duration between 5 minutes and 10 minutes at a temperature between 5 °C and 50 °C.

6. The manufacturing method according to claim 5, wherein the acidic solution is an aqueous solution containing 0.1 to 4 mol / L of protons.

7. The manufacturing method according to claim 1, wherein the ratio of nickel content by weight to phosphorus content by weight of the nickel-rich ash or the homogenate of nickel-rich biochar is less than 40.

8. The method according to claim 2, wherein the manufacturing of briquettes (16) comprises:a. manufacturing a mixture comprising the nickel-rich ash, as well as a binder, a source of reducing agent, a flux, and optionally additional materials providing alloying elements for the ferroalloy; andb. compressing this mixture to obtain the briquettes.

9. The method according to claim 8, wherein the additional materials come at least in part from sludge or dust from the metallurgical industry.

10. The manufacturing method according to claim 1, wherein the thermochemical treatment (14) is pyrolysis to obtain nickel-rich biochar, the method further comprising a step of grinding the biochar to obtain a homogenate of biochar.

11. The manufacturing method according to claim 10, wherein adjusting the phosphorus content comprises:a. mixing nickel-rich biochars from plants characterized by different combinations of species, geographical origins, and harvest years to obtain a predefined ratio of nickel content by weight to phosphorus content by weight in the mixture; and / orb. mixing the nickel-rich biochar with other nickel-containing materials to obtain in the mixture a value of the ratio of nickel content by weight to phosphorus content by weight greater than the value of the nickel content by weight to phosphorus content by weight in the nickel-rich biochar.

12. The method according to claim 10, wherein the manufacturing of briquettes comprises:manufacturing a mixture comprising the homogenate of nickel-rich biochar, as well as a binder, a flux, and additional materials providing alloying elements for the ferroalloy; andcompressing this mixture to obtain the briquettes.

13. The method according to claim 12, wherein the additional materials come at least in part from sludge or dust from the metallurgical industry.

14. The manufacturing method according to claim 1, wherein the plant material is provided in the form of a homogenate of plants, particularly in the form of granules comprising the homogenate of plants.

15. The manufacturing method according to claim 14, wherein the step of providing (12) plant material comprises:providing dried plants;grinding the dried plants to obtain a homogenate of plants; andoptionallycompressing this homogenate of plants to obtain granules.

16. The manufacturing method according to claim 15, further comprising, during the compression step to form the granules, heating the homogenate of plants to a temperature between 60 °C and 80 °C.

17. The manufacturing method according to claim 15, further comprising, during the compression step to form the granules, adding an adjuvant intended to facilitate the agglomeration of the homogenate of plants, the adjuvant being, preferably, water.

18. The method according to claim 1, wherein the plant material is obtained from nickel hyperaccumulator plants, for example, chosen from the following species:Odontarrhena chalcidica (syn=Alyssum murale)Bornmuellera emarginata (syn=Leptoplax emarginata)Bornmuellera tymphaea Berkheya coddii Blepharidium guatemalense Phyllanthus rufuschaneyi Rinorea aff. bengalensis.

19. The method according to claim 1, wherein adjusting the phosphorus content is carried out such that the briquettes have a ratio of nickel content by weight to phosphorus content by weight greater than or equal to 80.

20. The method according to claim 1, wherein the manufacturing (18) of the ferroalloy by pyrometallurgy from the briquettes comprises:introducing the briquettes into a furnace;melting the briquettes in the furnace to obtain a liquid ferroalloy, the ferroalloy comprising between 4% and 50% by weight of nickel andcasting the ferroalloy in the form of a semi-product, for example, in the form of ingots or granules.

21. The method according to claim 1, wherein the manufacturing (20) of stainless steel from the ferroalloy comprises:providing a mixture of the ferroalloy and scrap, the scrap comprising notably stainless steel scrap;melting this mixture in an electric furnace, particularly an electric arc furnace, to obtain a liquid steel; andrefining this liquid steel to obtain stainless steel.