Austenitic stainless steel containing nickel and molybdenum

Austenitic stainless steel with controlled chromium, manganese, nickel, carbon, nitrogen, and molybdenum composition addresses the high cost of nickel in conventional steels, achieving cost-effective cryogenic toughness and corrosion resistance.

US20260366120A1Pending Publication Date: 2026-11-19DOOSAN ENERBILITY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
US19/724888
Authority / Receiving Office
US · United States
Patent Type
Applications(United States)
Current Assignee / Owner
Priority Date
2024-01-15
Filing Date
2026-06-30
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Conventional austenitic stainless steels like STS 304 and STS 316 rely heavily on nickel, which is a high-cost commodity, and there is a need for alternative materials that offer superior cost competitiveness without compromising cryogenic performance and mechanical safety, while also maintaining resistance to corrosion-induced weight loss.

Method used

An austenitic stainless steel composition is developed with controlled amounts of chromium, manganese, nickel, carbon, nitrogen, and molybdenum, optimizing the balance to stabilize the austenite phase and enhance impact absorbed energy and pitting potential, using lower-cost elements like manganese and nitrogen as substitutes for nickel, and synergistic effects of nickel and molybdenum to improve corrosion resistance.

Benefits of technology

The new steel composition achieves enhanced cost-competitiveness, maintains a stable austenite phase from ambient to cryogenic temperatures, and exhibits excellent cryogenic toughness with impact absorbed energy of at least 41 J at -196 °C, along with improved pitting potential and corrosion resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure US20260366120A1-D00000_ABST
    Figure US20260366120A1-D00000_ABST
Patent Text Reader

Abstract

An austenitic stainless steel is provided. The austenitic stainless steel includes chromium (Cr), manganese (Mn), nickel (Ni), carbon (C), nitrogen (N), and molybdenum (Mo), with iron (Fe) and inevitable impurities as a balance. By incorporating low-cost manganese (Mn), carbon (C), and nitrogen (N) as interstitial alloying elements in a specific range, the austenitic stainless steel exhibits enhanced cost-competitiveness compared to conventional STS 304 and STS 316, while simultaneously maintaining a stable austenitic phase from ambient temperature down to cryogenic temperatures. The austenitic stainless steel further demonstrates excellent cryogenic toughness, with an impact absorbed energy of at least 41 J at an ultra-low temperature of −196 °C.
Need to check novelty before this filing date? Find Prior Art

Description

CROSS REFERENCE TO RELATED APPLICATION(S)

[0001] This application is a continuation application filed under 35 U.S.C. § 111(a) and claims the benefit under 35 U.S.C. §§ 120 and 365(c) of International Application No. PCT / KR2025 / 000907, filed on Jan. 15, 2025, which claims priority to Korean Patent Application No. 10-2024-0006023, filed on Jan. 15, 2024, the disclosures of which are incorporated herein by reference in their entireties.BACKGROUNDTechnical Field

[0002] Exemplary embodiments relate to an austenitic stainless steel containing nickel and molybdenum.Description of the Related Art

[0003] Conventional austenitic stainless steels, such as STS 304 and STS 316 materials, are widely utilized in liquefied natural gas (LNG) storage vessels because they maintain a stable austenite phase even at ultra-low or cryogenic temperatures. However, these conventional materials heavily rely on nickel (Ni) as a primary austenite-stabilizing alloying element. Because nickel is a high-cost commodity, its extensive inclusion imposes a significant economic burden on manufacturing.

[0004] Consequently, a need exists for alternative structural materials that offer superior cost competitiveness relative to STS 304 and STS 316 without compromising cryogenic performance. To achieve this, low-cost austenite-stabilizing elements—such as manganese (Mn), carbon (C), and nitrogen (N)—must be strategically alloyed to reduce the absolute nickel content while successfully maintaining a stable austenite single-phase microstructure at ambient and cryogenic temperatures.

[0005] Furthermore, under International Maritime Organization (IMO) regulations, structural materials designated for LNG vessel applications must meet stringent mechanical safety thresholds, including an impact absorbed energy of at least 41 J at a cryogenic temperature of −196 °C. Accordingly, there is a need to optimize the chemical composition of an austenitic stainless steel material that satisfies these strict cryogenic toughness requirements while concurrently exhibiting a resistance to corrosion-induced weight loss that is comparable or superior to that of conventional STS 304 and STS 316.SUMMARY

[0006] Aspects of one or more exemplary embodiments provide an austenitic stainless steel having improved impact absorbed energy and pitting potential through the incorporation of nickel and molybdenum.

[0007] Additional aspects will be set forth in part in the description which follows and, in part, will become apparent from the description, or may be learned by practice of the exemplary embodiments.

[0008] According to an aspect of an exemplary embodiment, there is provided an austenitic stainless steel, including: 16 to 20 wt. % of chromium (Cr); 4.5 to 9 wt. % of manganese (Mn); 3 to 6 wt. % of nickel (Ni); 0.05 to 0.3 wt. % of carbon (C); 0.1 to 0.35 wt. % of nitrogen (N); and more than 0 to 5.0 wt. % of molybdenum (Mo), with a balance being iron (Fe) and inevitable impurities.

[0009] A combined content of the nickel and the molybdenum (Ni+Mo) may be in a range of 4.0 to 7.0 wt. %.

[0010] The combined content of the nickel and the molybdenum (Ni+Mo) may be i range of 4.27 to less than 6.69 wt. %.

[0011] A pitting potential of the austenitic stainless steel may satisfy Equation 1 below:Epit=−0.04395(Ni+Mo)2+0.5834(Ni+Mo)−1.4916  [Equation 1]wherein, Epit represents the pitting potential, Ni represents the content of nickel in weight percent (wt. %), and Mo represents the content of molybdenum in weight percent (wt. %).The austenitic stainless steel may have an impact absorbed energy of equal to or greater than 41 J at a temperature of −196 °C.

[0013] The austenitic stainless steel may have a pitting potential (Epit) of equal to or greater than 0.2 VSCE.

[0014] The content of the chromium (Cr) may be in a range of 16.5 to 18.5 wt. %.

[0015] The content of the manganese (Mn) may be in a range of 6.0 to 8.0 wt. %.

[0016] The content of the nickel (Ni) may be in a range of 3.5 to 5.0 wt. %.

[0017] The content of the nitrogen (N) may be in a range of 0.15 to 0.28 wt. %.

[0018] The content of the molybdenum (Mo) may be in a range of 0.05 to 2.5 wt. %.

[0019] According to the present disclosure, an austenitic stainless steel provides several technical advantages. By incorporating low-cost manganese (Mn), carbon (C), and nitrogen (N) as interstitial alloying elements in a specific range, the austenitic stainless steel exhibits enhanced cost-competitiveness compared to conventional STS 304 and STS 316, while simultaneously maintaining a stable austenitic phase from ambient temperature down to cryogenic temperatures. The austenitic stainless steel further demonstrates excellent cryogenic toughness, with an impact absorbed energy of at least 41 J at an ultra-low temperature of −196 °C.BRIEF DESCRIPTION OF THE DRAWINGS

[0020] The above and other aspects will become more apparent from the following description of the exemplary embodiments with reference to the accompanying drawings, in which:

[0021] FIG. 1 is a graph illustrating polarization curves according to an exemplary embodiment;

[0022] FIG. 2 is a graph illustrating evaluation results of pitting potential according to an exemplary embodiment; and

[0023] FIG. 3 is a graph illustrating evaluation results of impact absorbed energy according to an exemplary embodiment.DETAILED DESCRIPTION

[0024] Various modifications and various embodiments will be described in detail with reference to the accompanying drawings so that those skilled in the art can easily carry out the disclosure. However, it is to be understood that the various embodiments are not limited to the scope of the disclosure to the specific exemplary embodiments, but they should be interpreted to include all modifications, equivalents, and substitutions of the embodiments included in the spirit and the scope disclosed herein. In the following description, like reference numerals refer to like components, even in different drawings. In certain embodiments, detailed descriptions of known functions and configurations which are deemed to make the gist of the present disclosure obscure will be omitted. For the same reason, some elements in the accompanying drawings may be exaggerated, omitted, or simplified.

[0025] Terms such as “first” and “second” may be used to describe various elements, but these elements should not be limited by these terms. These terms are only used to distinguish one element from another element. The use of such ordinal numbers should not be construed as limiting the meaning of the term. For instance, the elements associated with such an ordinal number should not be limited in the order of use, placement order, or the like. If necessary, each ordinal number may be used interchangeably.

[0026] Terms used herein are only for illustrative purposes of specific embodiments and are not intended to limit the present disclosure. The singular forms include the plural forms where not contrary to the context. It will be further understood that the terms such as “comprise”, “include”, and “have / has specify the presence of stated features, integers, steps, operations, elements, components, and / or combinations thereof but do not preclude the presence or addition of one or more other features, integers, steps, operations, elements, components, and / or combinations thereof.

[0027] Unless otherwise defined, all terms including technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the present disclosure belongs. It will be further understood that terms, such as those defined in commonly used dictionaries, may be interpreted as having meanings consistent with their ordinary meaning in the context of the relevant art, and will not be interpreted in an idealized or overly formal sense unless expressly defined otherwise herein.

[0028] An austenitic stainless steel according to an exemplary embodiment may include 16 to 20 wt. % of chromium (Cr), 4.5 to 9 wt. % of manganese (Mn), 3 to 6 wt. % of nickel (Ni), 0.05 to 0.3 wt. % of carbon (C), 0.1 to 0.35 wt. % of nitrogen (N), and greater than 0 to 5.0 wt. % of molybdenum (Mo), with the balance being iron (Fe) and inevitable impurities.

[0029] In one embodiment, the austenitic stainless steel may include the nickel and the molybdenum in a combined amount of 4.0 to 7.0 wt. %.

[0030] In one embodiment, the austenitic stainless steel may include the nickel and the molybdenum in a combined amount of 4.6 to less than 5.0 wt. %.

[0031] In one embodiment, the austenitic stainless steel may include the nickel and the molybdenum in a combined amount of 5.0 to 7.0 wt. %.

[0032] Hereinafter, reasons for the numerical limitations of the present disclosure will be described.(1) Chromium (Cr): In the Range of 16 to 20 wt. %

[0033] Chromium is an essential alloying element that imparts corrosion resistance t the austenitic stainless steel by forming a passive film on the alloy surface. To ensure sufficient corrosion resistance and structural integrity under aggressive operating environments, the austenitic stainless steel must include chromium in an amount of at least 16 wt. %. However, chromium acts as a ferrite-stabilizing element. If the chromium content exceeds 20 wt. %, the excessive chromium content can disrupt the phase stability of the alloy, promoting the precipitation of a sigma phase. The formation of the sigma phase drastically reduces localized corrosion resistance due to localized chromium depletion and severely compromises the cryogenic impact toughness of the material. Therefore, to balance passive film stability against the risk of deleterious phase precipitation, the austenitic stainless steel may include chromium in an amount of 16 to 20 wt. %. According to another exemplary embodiment, the content of chromium (Cr) may be tightly controlled within a narrower window to optimize both cost efficiency and structural phase stability. Specifically, the content of the chromium (Cr) may be maintained from 16.5 to 18.5 wt. %. Restricting the chromium content to this range ensures excellent basic corrosion resistance while reliably suppressing the formation of brittle delta-ferrite or sigma phases during hot-rolling or cryogenic deployment.(2) Manganese (Mn): In the Range of 4.5 to 9 wt. %

[0034] Manganese is a key alloying element that serves as an effective, low-cost substitute for nickel to stabilize the austenite phase. Additionally, manganese increases the solid solubility of nitrogen within the alloy matrix, thereby preventing nitrogen outgassing and stabilizing the microstructure. To achieve these austenite-stabilizing and nitrogen-retaining effects, the austenitic stainless steel must include manganese in an amount of at least 4.5 wt. %. However, when the manganese content exceeds 9 wt. %, excessive manganese may react with impurities such as sulfur(S) or oxygen (O) to form coarse non-metallic inclusions, such as manganese sulfides (MnS) or manganese oxides (MnO), which may degrade the corrosion resistance and mechanical properties of the austenitic stainless steel. Therefore, to suppress the formation of deleterious non-metallic inclusions while ensuring a stable austenitic phase, it is preferable that the austenitic stainless steel includes manganese in an amount of 4.5 to 9 wt. %. According to another exemplary embodiment, the content of manganese (Mn) may be adjusted to a narrower range of 6.0 to 8.0 wt. %. Maintaining the manganese content within this specific window provides a critical balance, ensuring sufficient stabilization of the austenitic phase and enhanced nitrogen solubility at a highly optimized raw material cost, without inducing segregation issues during ingot casting.(3) Nickel (Ni): In the Range of 3 to 6 wt. %

[0035] Nickel is a powerful austenite-stabilizing element that expands the austenite phase and significantly enhances the cryogenic toughness, ductility, and formability of the alloy. To ensure that the alloy achieves the required mechanical properties and exhibits sufficient impact absorbed energy at a cryogenic temperature of −196 °C, the austenitic stainless steel must include nickel in an amount of at least 3 wt. %. However, because nickel is a high-cost commodity element, excessive additions may significantly increase raw material and manufacturing costs, undermining the economic advantages of the alloy. Therefore, to maximize cryogenic impact toughness and general corrosion resistance while minimizing manufacturing expenditures, it is preferable that the austenitic stainless steel includes nickel in an amount of 3 to 6 wt. %. According to another exemplary embodiment, the content of nickel (Ni) may be restricted to a targeted sub-range of 3.5 to 5.0 wt. %. By pairing this lean nickel content with the controlled manganese, carbon, and nitrogen additions, the alloy successfully minimizes the utilization of expensive nickel while reliably preserving excellent structural stability, high impact toughness, and fracture resistance at ultra-low temperatures.(4) Carbon (C): In the Range of 0.05 to 0.3 wt. %

[0036] Carbon is an alloying element that significantly contributes to the stabilization of the austenite phase and suppresses deformation-induced martensitic transformation under cryogenic strain. To ensure sufficient phase stability and adequate base mechanical strength, the austenitic stainless steel must include carbon in an amount of at least 0.05 wt. %. However, when the carbon content exceeds 0.3 wt. %, the excessive carbon may promote the formation of carbides, which may reduce corrosion resistance. Therefore, to suppress grain-boundary sensitization while retaining strong austenite stabilization, it is preferable that the austenitic stainless steel includes carbon in an amount of 0.05 to 0.3 wt. %.(5) Nitrogen (N): In the Range of 0.1 to 0.35 wt. %

[0037] Nitrogen is an effective interstitial alloying element that acts as a powerful austenite stabilizer, serving as an efficient and cost-effective partial substitute for nickel. To ensure sufficient matrix stabilization and to achieve a high resistance to localized corrosion, the austenitic stainless steel must include nitrogen in an amount of at least 0.1 wt. %. However, when the nitrogen content exceeds 0.35 wt. %, the excessive nitrogen may promote the formation of nitrides, which may reduce corrosion resistance and toughness. Therefore, to maximize solid-solution strengthening and phase stability while avoiding harmful nitride precipitation or casting defects, it is preferable that the austenitic stainless steel includes nitrogen in an amount of 0.1 to 0.35 wt. %. According to another exemplary embodiment, the content of nitrogen (N) may be selectively maintained in a range of 0.15 to 0.28 wt. %. Controlling the nitrogen content within this optimum range enhances the interstitial solid-solution strengthening effect and improves localized corrosion resistance, while effectively preventing the formation of deleterious nitride precipitates or gas porosity during solidification.(6) Molybdenum (Mo): Greater than 0 to 5.0 wt. %

[0038] Molybdenum is an optional element that improves localized corrosion resistance by forming a passive oxide on the surface of stainless steel. However, excessive molybdenum content exceeding 5.0 wt. % may promote the formation of a sigma phase, which may deteriorate the impact absorbed energy at −196 °C. Therefore, when molybdenum is added, the austenitic stainless steel preferably includes molybdenum in an amount of greater than 0 and less than or equal to 5.0 wt. %. According to another exemplary embodiment, the content of molybdenum (Mo) may be adjusted within a narrower range of 0.05 to 2.5 wt. %. When constrained to this specific window, the molybdenum works synergistically with the nickel and nitrogen to markedly elevate the pitting potential (Epit) of the alloy in chloride environments, while remaining below the threshold where detrimental intermetallic phases might precipitate.(7) Combined Nickel and Molybdenum (Ni+Mo): In the Range of 4.0 to 7.0 wt. %

[0039] Nickel and molybdenum may interact synergistically to significantly elevate the pitting potential and localized corrosion resistance of the austenitic stainless steel. For example, when molybdenum is added in isolation to a manganese-nitrogen bearing austenitic stainless steel, no significant change in pitting potential is observed. On the contrary, when molybdenum is co-alloyed alongside nickel to a manganese-nitrogen bearing austenitic stainless steel, the pitting potential increases significantly. This empirical divergence demonstrates that the interaction between nickel and molybdenum actively suppresses localized pitting propagation. Accordingly, to optimize this synergistic effect while balancing raw material costs, the combined content of nickel and molybdenum (Ni+Mo) is strictly controlled to a range of 4.0 wt. % to 7.0 wt. %, and more preferably to a sub-range of 4.5 wt. % to 6.5 wt. %.

[0040] When the combined content of nickel and molybdenum (Ni+Mo) is less than 4.0 wt. %, the structural stability of the austenitic phase is compromised at cryogenic temperatures, causing the impact absorbed energy at −196 °C to drop below the critical threshold of 41 J. On the other hand, when the combined content of nickel and molybdenum exceeds 7.0 wt. %, the raw material and manufacturing costs prohibitively increase because both nickel and molybdenum are expensive alloying elements, thereby undermining the cost-competitiveness of the alloy without providing a corresponding, economically justifiable increase in performance. Accordingly, the combined content of nickel and molybdenum is bounded by the specified range to simultaneously ensure exceptional cryogenic toughness and cost-effective commercial viability.

[0041] In one embodiment, the pitting potential of the austenitic stainless steel containing nickel and molybdenum in a combined amount of 4.0 to 7.0 wt. % may satisfy Equation 1 below:Epit=−0.04395(Ni+Mo)2+0.5834(Ni+Mo)−1.4916  [Equation 1]in Equation 1, Epit represents the pitting potential, Ni represents the content of nickel in weight percent (wt. %), and Mo represents the content of molybdenum in weight percent (wt. %).In one embodiment, the austenitic stainless steel exhibits a Charpy V-notch impact absorbed energy of equal to or greater than 41 J at a cryogenic temperature of −196 °C. When the impact absorbed energy is less than about 41 J at −196 °C, the alloy fails to satisfy the stringent structural toughness requirements mandated for cryogenic structural components, rendering the material unsuitable for deployment in LNG containment vessels.

[0043] In one embodiment, the austenitic stainless steel exhibits a pitting potential of equal to or greater than 0.2 VSCE, thereby ensuring high resistance to localized pitting corrosion in chloride-containing environments.

[0044] The following Examples are provided to illustrate specific embodiments of the present disclosure in further detail. However, it should be understood by those skilled in the art that these Examples are merely illustrative, exemplary, and non-exhaustive in nature. The specific technical configurations, chemical compositions, processing parameters, and experimental results described below do not limit the scope of the present disclosure. Thus, the Examples are provided to enable to those skilled in the art to fully understand and practice the present disclosure.EXAMPLE 1

[0045] Nitrogen gas was introduced into a vacuum induction melting (VIM) furnace, and commercially available electrolytic iron, chromium, manganese, nickel, molybdenum, and carbon powder, each having a purity of 95% or higher, were melted utilizing a master alloy. The resulting melt was cast to fabricate a laboratory-scale steel ingot. The steel ingot was subsequently soaked, heated to a target temperature of 1200 °C for a predetermined duration, and then hot-rolled into a structural plate having a nominal thickness of 11.5 mm. In this exemplary embodiment, the combined content of nitrogen and molybdenum (Ni+Mo) was controlled to 4.35 wt. %.EXAMPLE 2

[0046] A laboratory-scale steel ingot was manufactured in the same manner as described in Example 1, except that the combined content of nickel and molybdenum (Ni+Mo) was adjusted to 4.606 wt. %.EXAMPLE 3

[0047] A laboratory-scale steel ingot was manufactured in the same manner as described in Example 1, except that the combined content of nickel and molybdenum (Ni+Mo) was adjusted to 4.766 wt. %.EXAMPLE 4

[0048] A laboratory-scale steel ingot was manufactured in the same manner as described in Example 1, except that the combined content of nickel and molybdenum (Ni+Mo) was adjusted to 5.01 wt. %.EXAMPLE 5

[0049] A laboratory-scale steel ingot was manufactured in the same manner as described in Example 1, except that the combined content of nickel and molybdenum (Ni+Mo) was adjusted to 5.21 wt. %.EXAMPLE 6

[0050] A laboratory-scale steel ingot was manufactured in the same manner as described in Example 1, except that the combined content of nickel and molybdenum (Ni+Mo) was adjusted to 5.353 wt. %.EXAMPLE 7

[0051] A laboratory-scale steel ingot was manufactured in the same manner as described in Example 1, except that the combined content of nickel and molybdenum (Ni+Mo) was adjusted to 5.36 wt. %.EXAMPLE 8

[0052] A laboratory-scale steel ingot was manufactured in the same manner as described in Example 1, except that the combined content of nickel and molybdenum (Ni+Mo) was adjusted to about 6.692 wt. %.Comparative Example 1

[0053] A commercially available STS 304 was prepared to serve as a baseline comparative reference material.Comparative Example 2

[0054] A commercially available STS 316 was prepared to serve as a baseline comparative reference material.Experimental Example 1

[0055] FIG. 1 is a graph illustrating potentiodynamic polarization curves for the austenitic stainless steel compositions according to an exemplary embodiment. To evaluate localized corrosion resistance, potentiodynamic polarization measurements were conducted at an ambient temperature of 25 °C in an aqueous electrolyte solution containing 3.5 wt. % sodium chloride (NaCl). The polarization curves were recorded at a constant potential scan rate of about 0.2 mV / s utilizing a Gamry Reference 600 potentiostat. As used herein, the pitting potential (Epit) is defined as the electrochemical potential threshold at which localized breakdown of the passive film occurs and stable pitting corrosion initiates on the surface of the austenitic stainless steel. Accordingly, a higher pitting potential value indicates a greater resistance to, and delay in, the initiation of pitting corrosion. The polarization data confirmed that both the Examples and Comparative Examples exhibited well-defined passive regions and stable passive behavior under the tested conditions.

[0056] FIG. 2 is a graph illustrating the evaluation results of pitting potential as a function of the combined content of nickel and molybdenum (Ni+Mo) according to an exemplary embodiment. As illustrated in FIG. 2, the pitting potential of Comparative Example 1 was determined to be 0.3 VSCE, whereas the pitting potential of Comparative Example 2 fell within a range of 0.35 to 0.41 VSCE. In contrast, for the Examples, when the combined content of nickel and molybdenum (Ni+Mo) was equal to or greater than 4.766 wt. %, the resulting pitting potential values were equal to or higher than 0.3 VSCE baseline of Comparative Example 1. Furthermore, when the combined content of nickel and molybdenum (Ni+Mo) was increased to equal to or greater than 5.353 wt. %, the pitting potential values were equal to or higher than the superior 0.35 to 0.41 VSCE baseline of Comparative Example 2. Additionally, when the combined content of nickel and molybdenum (Ni+Mo) was maintained within the range of 4.27 to 6.69 wt. %, the measured pitting potentials cleanly satisfied Equation 1 below:Epit=−0.04395(Ni+Mo)2+0.5834(Ni+Mo)−1.4916  [Equation 1]in Equation 1, Epit represents the pitting potential, Ni represents the content of nickel in weight percent (wt. %), and Mo represents the content of molybdenum in weight percent (wt. %).FIG. 3 is a graph illustrating the evaluation results of Charpy impact absorbed energy at a cryogenic temperature of −196 °C for the austenitic stainless steel according to an exemplary embodiment. The impact absorbed energy was measured utilizing a Charpy impact tester (Tinius Olsen, Model IT542E) in accordance with the standardized testing procedures specified in ASTM A370 for the impact testing of metallic materials. For structural application in LNG containment vessels, a Charpy V-notch impact absorbed energy of at least 41 J at an ultra-low temperature of −196 °C is strictly required to ensure adequate resistance to brittle fracture. As demonstrated in FIG. 3, each of Examples 1 to 8 successfully exhibited a Charpy V-notch impact absorbed energy values that exceeded the critical 41 J threshold at −196 °C.

[0058] While one or more exemplary embodiments have been described with reference to the accompanying drawings, it will be understood by those skilled in the art that various modifications in form and details may be made therein without departing from the idea and scope as defined in the appended claims.

Claims

1. An austenitic stainless steel, comprising:16 to 20 wt. % of chromium (Cr);4.5 to 9 wt. % of manganese (Mn);3 to 6 wt. % of nickel (Ni);0.05 to 0.3 wt. % of carbon (C);0.1 to 0.35 wt. % of nitrogen (N); andmore than 0 to 5.0 wt. % of molybdenum (Mo),with a balance being iron (Fe) and inevitable impurities.

2. The austenitic stainless steel of claim 1, wherein a combined content of the nickel and the molybdenum (Ni+Mo) is in a range of 4.0 to 7.0 wt. %.

3. The austenitic stainless steel of claim 2, wherein the combined content of the nickel and the molybdenum (Ni+Mo) is in a range of 4.27 to less than 6.69 wt. %.

4. The austenitic stainless steel of claim 2, wherein a pitting potential of the austenitic stainless steel satisfies Equation 1 below:Epit=−0.04395(Ni+Mo)2+0.5834(Ni+Mo)−1.4916  [Equation 1]wherein, Epit represents the pitting potential, Ni represents the content of nickel in weight percent (wt. %), and Mo represents the content of molybdenum in weight percent (wt. %).

5. The austenitic stainless steel of claim 1, wherein the austenitic stainless steel has an impact absorbed energy of equal to or greater than 41 J at a temperature of −196 °C.

6. The austenitic stainless steel of claim 1, wherein the austenitic stainless steel has a pitting potential (Epit) of equal to or greater than 0.2 VSCE.

7. The austenitic stainless steel of claim 1, wherein the content of the chromium (Cr) is in a range of 16.5 to 18.5 wt. %.

8. The austenitic stainless steel of claim 1, wherein the content of the manganese (Mn) is in a range of 6.0 to 8.0 wt. %.

9. The austenitic stainless steel of claim 1, wherein the content of the nickel (Ni) is in a range of 3.5 to 5.0 wt. %.

10. The austenitic stainless steel of claim 1, wherein the content of the nitrogen (N) is in a range of 0.15 to 0.28 wt. %.

11. The austenitic stainless steel of claim 1, wherein the content of the molybdenum (Mo) is in a range of 0.05 to 2.5 wt. %.