Aluminum-based member and method for producing same
An anodized film with straight tube-shaped main pores and sidewall sub-pores addresses the need for improved adhesion and resistance by allowing better penetration and engagement of upper layers, enhancing flexibility and thermal resistance.
Patent Information
- Application Number
- US19/154257
- Authority / Receiving Office
- US · United States
- Patent Type
- Applications(United States)
- Current Assignee / Owner
- Priority Date
- 2023-02-06
- Filing Date
- 2023-11-07
- Publication Date
- 2026-11-19
AI Technical Summary
Existing anodized films on aluminum-based members lack a novel form that enhances adhesion and bonding properties of upper layers while providing impact and thermal resistance.
An anodized film with main pores extending in an approximately straight tube shape and sub-pores opening on the sidewalls, offering a porosity of 18% to 65%, which allows for improved penetration and engagement of upper layers and increased flexibility.
The anodized film exhibits excellent adhesion and bonding properties with upper layers, along with enhanced impact and thermal resistance due to its unique pore structure.
Smart Images

Figure US20260366186A1-D00000_ABST
Abstract
Description
TECHNICAL FIELD
[0001] The present invention relates to an aluminum-based member having an anodized film on at least a portion of its surface.BACKGROUND ART
[0002] Aluminum-based members (Al-based members) are subjected to anodization treatment for the purpose of ensuring corrosion resistance, insulation, etc. Anodization treatment is performed by energization using an aluminum base material (Al base material) immersed or the like in an electrolytic solution bath (such as a sulfuric acid bath or an oxalic acid bath) as the positive electrode (anode). This allows an anodized film (alumite film) composed of aluminum oxide (such as Al2O3) to be formed on the surface (treated surface) of the Al base material. Anodization treatment differs from plating and other treatments in that it involves oxidation of the Al base material itself.
[0003] Anodized films are usually composed of a dense and thin barrier layer (active layer) and a porous layer (growth layer) grown on top of it. In general anodized films, the majority of the film is made up of a porous layer composed of approximately straight tube-shaped (cylindrical) micropores (groups) that open on the surface side. Anodized films, which are intended to improve corrosion resistance, can also be treated to seal the openings in the porous layer or to fill the pores.
[0004] Meanwhile, in addition to ensuring the corrosion resistance, anodized films are also used as lower layers (bases) that ensure the adhesion and bonding properties, etc. of upper layers (e.g., resin layers such as coating films) formed on the surfaces. Descriptions related to such anodized films are found, for example, in the following patent documents.PRIOR ART DOCUMENTSPatent DocumentsPatent Document 1: U.S. Pat. No. 4,085,012A
[0006] Patent Document 2: JP2008-13805A
[0007] Patent Document 3: JP2013-76118A
[0008] Patent Document 4: JP2021-75763ASUMMARY OF INVENTIONTechnical Problem
[0009] Patent document 1 discloses that an anodized film is formed by energizing (3 to 25 V) pure aluminum in contact with an electrolytic solution (65 °F to 95 °F / 18 °C to 35 °C) containing phosphoric acid (3% to 20%) (see TABLE 1 of Patent Document 1). Patent document 1 does not describe the form of the anodized film.
[0010] Patent Document 2 discloses that an anodized film containing organic compound components is formed by energizing (2 A / dm2, 14 V) an Al—Mn-based base material (A3004) in contact with an electrolytic solution (50 °C) containing sodium phosphate (5 wt %) and tannic acid (1.25 wt %). This anodized film has a thickness of 20 nm, a water content of 2%, and a porosity of 3%, and is very thin and dense overall (see Example 5 of Patent Document 2).
[0011] Patent Document 3 discloses that an anodized film is formed by energizing (2 to 4 A / cm2, 20 to 80 V) an Al—Mg—Si-based base material (A6061) in contact with an electrolytic solution (15 °C to 25 °C) composed of an aqueous phosphoric acid solution (20 wt %). This anodized film has columnar cells, which are composed of pores extending in the axial direction, and branch pores, which extend vertically from the inner peripheral surface (see FIG. 1 of Patent Document 3). Patent Document 3, however, does not include any microscopic photographs or the like, and the specific form is unknown. Since the base material containing Si is subjected to anodization treatment, it is inferred that the branch pores are very small to such an extent that they are formed in the process in which the porous layer avoids the Si and grows.
[0012] Patent Document 4 discloses that a first oxide film is formed by energizing (15 V) an Al—Mg-based base material (A5052) in contact with an electrolytic solution (15 °C) composed of an aqueous phosphoric acid solution (1.46 mol / L) and then a second oxide film is further formed by energizing (12.5 V) the base material in contact with an electrolytic solution (20 °C to 23 °C) composed of an aqueous sulfuric acid solution (3.67 mol / L). The film thus formed has a complex shape that differs from an anodized film having fine pores extending in an approximately straight tube shape (see FIG. 3 of Patent Document 4).
[0013] The present invention has been made in view of such circumstances, and an object of the present invention is to provide an aluminum-based member having an anodized film of a novel form and relevant techniques.Solution to Problem
[0014] As a result of intensive studies to achieve the above object, the present inventors have succeeded in forming an anodized film having sub-pores penetrating the side walls of main pores extending in an approximately straight tube shape. Developing this achievement, the present inventors have accomplished the present invention, which will be described below.«Aluminum-Based Member»
[0015] (1) The aluminum-based member (also referred to as an “Al-based member”) of the present invention is an aluminum-based member in which at least part of a surface of an aluminum base material is coated with an anodized film, wherein the anodized film has main pores that extend in an approximately straight tube shape from the aluminum base material side and sub-pores that open on some of sidewalls of the main pores, and the anodized film has a porosity of 18% to 65% when determined by observing a top surface of the anodized film.
[0016] (2) The anodized film according to the present invention has a large overall porosity, and in addition to the main pores that extend in an approximately straight tube shape, it also has sub-pores that open on the side walls of the main pores. Therefore, when an upper layer (e.g., a resin layer) is formed on the anodized film, for example, the components (such as resin) of the upper layer may readily undergo penetration, filling, engagement, etc. not only into the main pores but also into the sub-pores, and it is expected that the adhesion and bonding properties, etc. of the upper layer can be improved due to an increased anchor effect.
[0017] Moreover, the anodized film according to the present invention has sub-pores in addition to the main pores and has a high porosity, so it is highly flexible. Such an anodized film is less likely to generate breakage (crack) or the like even when subjected to impact, thermal stress, etc., and can exhibit excellent properties such as impact resistance and heat resistance.«Method for Producing an Aluminum-Based Member, Etc.»
[0018] The present invention may also be perceived as a method for producing an aluminum-based member or an anodization method. For example, the present invention may be a method for producing an aluminum-based member, comprising an electrolytic step of energizing an aluminum base material that is in contact with an electrolytic solution containing phosphoric acid, wherein the above-described aluminum-based member is obtained.
[0019] When the electrolytic solution contains phosphoric acid, the formation of the above-described anodized film is promoted, and the surface of the anodized film can be coated with an insoluble phosphate film. The phosphate film inhibits the natural sealing of the anodized film (hydration reaction with moisture contained in the air). Therefore, even if the anodized film is left in the air for a long time, the opening state of the main pores and sub-pores is maintained, and the function of the anodized film as a base layer can be stably ensured.«Others»
[0020] (1) In the present specification, for descriptive purposes, the outermost surface side of the anodized film (the opening side of the main pores) is referred to as the upper side or top side. Conversely, the opposite side (the Al base material side) is referred to as the lower side or bottom side. As appropriate, the film thickness direction of the anodized film (usually the growth direction of the main pores) is also referred to as the vertical direction, and the direction approximately perpendicular to that is also referred to as the horizontal direction.
[0021] The porosity and opening diameter are evaluated based on the image (observation image) obtained by observing the top side of the anodized film with a microscope. The presence or absence (number) and form of the sub-pores can also be evaluated based on the observation image of the top side, but it may be preferably evaluated based on the observation image of the side (cross-sectional) surface of the anodized film (longitudinal cross section obtained by cutting in the film thickness direction). The sub-pores may be preferably evaluated at least in the surface region (depth 1 μm×width 10 μm) near the outermost surface of the anodized film.
[0022] The evaluation of the observation image may be preferably performed, for example, using image analysis software. The number (distribution) of sub-pores may also be counted visually based on the observation image.
[0023] The field of view (evaluation range) of the observation image is not limited, but it may be, for example, 0.6 μm×0.5 μm to 12.7 μm×8.8 μm.
[0024] Porosity is the ratio of the pore area (total value) to the total area of the anodized film within the observed field of view. Opening diameter is the arithmetic mean value of the circle equivalent diameter of each pore within the same field of view. Porosity and opening diameter are calculated, for example, using image analysis software (Image J).
[0025] Unless otherwise stated, the film thickness of the anodized film is the measured value using a film thickness meter. If appropriate, the film thickness may be the distance (average value) from the bottom surface of the anodized film (the lowermost surface of the barrier layer) to the outermost surface (the top surface of the porous layer) based on the observation image.
[0026] (2) Unless otherwise stated, a numerical range “x to y” as referred to in the present specification includes the lower limit x and the upper limit y. Any numerical value included in various numerical values or numerical ranges described in the present specification may be selected or extracted as a new lower or upper limit, and any numerical range such as “a to b” can thereby be newly provided using such a new lower or upper limit.BRIEF DESCRIPTION OF DRAWINGS
[0027] FIG. 1 is a set of SEM images when observing the top surfaces of anodized films according to First Example.
[0028] FIG. 2A is a set of SEM images when observing the upper sides of side cross-sections of the anodized films.
[0029] FIG. 2B is a set of SEM images when observing the lower sides (bottom sides) of side cross-sections of the anodized films.
[0030] FIG. 3A is a set of SEM images when observing the upper sides of side cross-sections of the anodized films according to Second Example.
[0031] FIG. 3B is a set of SEM images when observing the lower sides (bottom sides) of side cross-sections of the anodized films.
[0032] FIG. 4A is a set of SEM images when observing the top surfaces of anodized films according to Third Example.
[0033] FIG. 4B is a set of SEM images when observing the top surfaces of anodized films according to Third Example.EMBODIMENTS FOR CARRYING OUT THE INVENTION
[0034] The contents described in the present specification can apply not only to the products (such as an Al-based member and an anodized film) of the present invention, but also to the methods (such as a method for producing an Al-based member and an anodization method) as appropriate. One or more features freely selected from the present specification can be added to the features of the present invention. Which embodiment is the best or not is different depending on objectives, required performance, and other factors.«Anodized Film»
[0035] The anodized film has main pores that extend in an approximately straight tube shape from the Al base material side and sub-pores that open on some of sidewalls of the main pores(1) Main Pores
[0036] The main pores are, for example, bottomed tubular extending from the bottom portion of the Al base material side to the openings at the top portion. The pore form (shape, size) may vary slightly along the vertical direction (depth direction, axial direction, or extension direction).
[0037] The opening diameter of the main pores is, for example, 50 to 1000 nm, 100 to 500 nm, or 150 to 350 nm. Such an opening diameter tends to be larger than conventional columnar pores (cells).(2) Sub-Pores
[0038] The sub-pores open at some of the side walls of the main pores and extend in the horizontal direction (the direction approximately perpendicular to the side walls of the main pores). At least some of the sub-pores may penetrate the side walls of the main pores (communicate between adjacent main pores).
[0039] The distribution of the sub-pores may be uniform or non-uniform along the vertical direction of the main pores. When the sub-pores are larger on the upper side (opening side) than on the bottom side of the main pores, the anchor effect, etc. on the upper layer provided on the surface of the anodized film can be increased.
[0040] It is sufficient that at least one sub-pore is present in the field of view when the anodized film is observed from the side. Furthermore, it is preferred that there be at least one surface region (depth 1 μm×width 10 μm) containing one or more sub-pores in an embodiment, three or more sub-pores in another embodiment, or five or more sub-pores in still another embodiment.(3) Porosity
[0041] The porosity determined by observing the top surface of the anodized film is, for example, 18% to 65%, 20% to 55%, 25% to 50%, 30% to 45%, or 35% to 40%. Such porosity tends to be greater than that of conventional porous layers composed of columnar pores (cells). This is believed to allow the anodized film of the present invention to exhibit excellent flexibility (crack resistance), adhesion and bonding properties, etc. to upper layers.(4) Film Thickness
[0042] The anodized film has a film thickness, for example, of 0.1 to 20 μm, 0.5 to 10 μm, or 1 to 5 μm. The film thickness of the anodized film includes the thickness of the so-called barrier layer. The thickness of the barrier layer is, for example, 10 to 1000 nm, 50 to 500 nm, or 100 to 300 nm. The group of main pores formed on the barrier layer is also referred to as a “porous layer” in the present specification as appropriate.(5) Components
[0043] The anodized film is mainly composed of aluminum oxide (Al2O3), but may contain components derived from the composition of the electrolytic solution. For example, when an electrolytic solution containing phosphoric acid is used, P, H, etc. may be contained in the anodized film. In addition, phosphates (e.g., Al—P—O compounds, Al—P—O—H compounds), etc. may be present near the surface of the anodized film.«Al Base Material»
[0044] Provided that an anodized film having main pores and sub-pores is formed, the Al base material may be selected according to the application of the Al-based member. Representative Al base materials include, for example, pure aluminum (JIS A1000 series) whose Al content relative to the whole is 98 mass % or more in an embodiment, 98.5 mass % or more in another embodiment, 99 mass % or more in still another embodiment, or 99.6 mass % or more in yet another embodiment. When the Al-based member is an electrically-conductive member, it is preferred to use an Al base material whose electric conductivity is 50% IACS (International Annealed Copper Standard) or more in an embodiment, 55% IACS or more in another embodiment, or 60% IACS or more in still another embodiment. The unit “% IACS” refers to a relative index (ratio) to the electric conductivity (100% IACS) of annealed standard soft copper (volume resistivity: 1.7241×10−8 Ωm).
[0045] The Al base material may be, for example, any of a wrought material, a cast material, a plastically processed material, a sprayed material, etc. The Al base material may contain a small amount of a modifier element such as Mg, Fe, or Si (e.g., 1 mass % or less in an embodiment or 0.5 mass % or less in another embodiment in total) to improve the mechanical properties, etc.«Adherend»
[0046] An adherend may be present on at least a part of the anodized film. The adherend may be, for example, any of a resin body, a ceramic body, a metal body, etc. The adherend may be layered (including film-like) or block-like (bulk-like). In the case of a resin body, examples include a resin layer such as a coating film, a sealant, and an adhesive material. In the present specification, the adherend provided on the surface of the anodized film is referred to as an “upper layer” as appropriate, regardless of its form.«Production Method / Anodization Method»
[0047] The anodized film is formed by an electrolytic step of energizing an aluminum base material that is in contact with an electrolytic solution.(1) Electrolytic Solution
[0048] Provided that main pores and sub-pores are formed, the components of the electrolytic solution are not limited. The electrolytic solution may be, for example, an inorganic acid solution (phosphoric acid solution, sulfuric acid solution, chromic acid solution, etc.) or an organic acid solution (oxalic acid solution, etc.).
[0049] When an electrolytic solution containing phosphoric acid is used, the phosphoric acid concentration may be, for example, 1% to 30%, 2% to 20%, or 3% to 10%. The concentration of an electrolytic solution as referred to in the present specification is a mass ratio to the entire electrolytic solution unless otherwise stated. The temperature (bath temperature) of the electrolytic solution may be, for example, 15 °C to 80 °C, 20 °C to 60 °C, or 25 °C to 40 °C.(2) Energization
[0050] The electrolytic step is performed, for example, by constant current energization or constant voltage energization. The current (density) or applied voltage may vary (fluctuate) during the energization. The electrolytic step may be performed by DC energization, AC energization, or superimposed AC / DC energization combining AC and DC components. The waveform of the AC current may be a sine wave, a square wave, a pulse wave, or the like.
[0051] When the electrolytic step is performed by DC energization, for example, a high voltage of about 30 to 250 V in an embodiment, 40 to 200 V in another embodiment, or 75 to 175 V in still another embodiment may be applied to the Al base material at least temporarily. Any counter electrode may be placed in the electrolytic solution, but usually a platinum electrode or graphite electrode is used.«Applications»
[0052] The Al-based member may be used in any application. When the anodized film is used as an insulating coating or a part of it, the Al-based member may be an electrically-conductive member (wire, element, etc.). In this case, another insulator may be applied to the anodized film. For example, a resin layer (insulating layer) composed of insulating resin (enamel material) such as polyimide, polyurethane, or epoxy may be provided on the anodized film. The resin layer may contain a filler. Examples of the filler include a thermally conductive filler, a surge-resistant filler, and a dielectric constant-reducing filler.EXAMPLES
[0053] Several types of samples (Al-based members) were produced by performing various anodizing treatments under different conditions, with anodized films formed on the surfaces of the Al-based materials. The present invention will be described in more detail below with reference to these specific examples.First Example / Constant Current Electrolysis«Production of Samples»(1) Al Base Material
[0054] Test pieces (50 mm square×2 mm thick) composed of pure aluminum (JIS A1050) were prepared as the Al base materials to be subjected to anodization treatment.(2) Electrolytic Step
[0055] An electrolytic step was performed on the test pieces under the conditions listed in Table 1. An aqueous solution of phosphoric acid, sulfuric acid, or oxalic acid was used as the electrolytic solution. The concentrations listed in Table 1 are the mass ratios to the entire aqueous solution.
[0056] Each entire test piece was immersed in a treatment bath containing an electrolytic solution, and constant current (density) DC energization was performed for the test piece as the anode and a platinum electrode as the cathode while stirring the electrolytic solution. The current density listed in Table 1 is a value obtained by dividing the applied current value by the treated area of the test piece. The test piece was masked and only a part of its surface (24 cm2) was treated.
[0057] The applied voltage during the electrolytic step varies, but for reference, the measured voltage 10 minutes after the start of energization is also listed in Table 1.(3)
[0058] After the electrolytic step, the test piece taken out of the electrolytic solution was washed thoroughly with distilled water, sprayed with compressed air to remove moisture, and then dried thoroughly in the air. The anodized test pieces (samples 1, A1, and B1) thus obtained were subjected to the measurements and observations described below.«Measurements / Observations»(1) Film Thickness
[0059] The anodized surface of each sample (simply referred to as the “treated surface”) was measured using an eddy current film thickness meter (SWT-9200, available from SANKO ELECTRONIC LABORATORY CO., LTD.). The film thicknesses obtained are also listed in Table 1.(2) Surface Observation
[0060] The treated surface (surface / top surface) of each sample was observed using a scanning electron microscope (SEM / S-5500, available from Hitachi High-Tech Corporation). The SEM images obtained are collectively shown in FIG. 1.(3) Cross-Sectional Observation
[0061] The longitudinal section (side cross-section) of each sample was observed using the SEM in the same manner. The SEM images obtained are collectively shown in FIGS. 2A and 2B (collectively referred to as “FIG. 2”). FIG. 2A shows the upper side (surface side) near the treated surface, and FIG. 2B shows the lower side (bottom side).«Image Analysis»(1) Porosity
[0062] The porosity of each sample was determined by image analysis using ImageJ (free software) based on the SEM image (see FIG. 1) of the treated surface (top surface). The arithmetic mean value of the porosity of five randomly selected fields of view is also listed in Table 1.
[0063] In this analysis, the field of view of Sample 1 was 1280 nm×890 nm, and the field of view of Samples A1 and B1 was 640 nm×445 nm. The size of each field of view was adjusted so that each field of view would contain 10 or more main pores.
[0064] The porosity was determined as follows. First, the image to be analyzed was converted to 8 bits, and then binarized to extract the pores that were open on the surface. Then, after each pore was processed using the watershed algorithm, the total value of opening areas of pores with an opening area of 100 nm2 or more was calculated. The ratio of the total value of opening areas to the whole area of the field of view was defined as the porosity.(2) Opening Diameter
[0065] The same image analysis was performed based on the SEM image of the treated surface (top surface) to determine the opening diameter of each sample. Likewise, the arithmetic mean value of the opening diameter for five fields of view is also listed in Table 1. The opening diameter was determined as follows. First, as described above, the total value of opening areas of the extracted pores was divided by the number of extracted pores to determine the average opening area. The equivalent circle diameter (diameter when the pore was assumed to be a perfect circle) calculated from the average opening area was defined as the opening diameter. Note that the image of Sample 1 contains sub-pores in addition to the main pores, so the maximum diameter (maximum length) of 10 arbitrary main pores was measured, and the arithmetic mean value was defined as the opening diameter.«Evaluation»(1) Anodized Film
[0066] As can be seen from Table 1, Sample 1, which was subjected to the electrolytic step by applying a high voltage in an electrolytic solution containing phosphoric acid, had significantly larger porosity and opening diameter than the other samples. As can be seen from FIGS. 1 and 2, in addition to the thick main pores extending in an approximately straight tube shape from the Al base material side, the anodized film of Sample 1 also had many thin sub-pores that opened by cutting into the side walls of the main pores. This type of anodized film had a unique shape not seen in the anodized films of other samples.(2) Sub-Pores
[0067] As can be seen from FIG. 2A, the anodized film of Sample 1 was formed with a plurality of (approximately 10) sub-pores in the surface region (depth 1 μm×width 10 μm). Furthermore, as can be seen from the comparison of FIG. 2A and FIG. 2B, the sub-pores were larger in the upper layer region of the anodized film than in the lower layer region (bottom side, barrier layer side). Moreover, the density of the sub-pores tended to increase from the bottom to the top of the anodized film.Second Example / Upper Layer«Production of Samples»
[0068] As in First Example, the anodization treatment as listed in Table 2 was performed. After repeatedly spraying polyimide varnish onto the obtained anodized film (application step), it was further heated in a furnace (350 °C×1 hour) (thermal curing step). The test pieces (Samples 2, A2, and B2) in which a resin layer (upper layer) was thus attached onto the anodized film were subjected to the measurements and observations described below.«Measurements / Observations»(1) Film Thickness
[0069] The film thickness of the resin layer of each sample was measured using the above-described eddy current film thickness meter. The results are also listed in Table 2. The film thickness of the anodized film itself, measured prior to the application step, is also listed in Table 2. The film thickness of the resin layer was determined by subtracting the film thickness of the anodized film alone from the overall thickness after the resin layer was formed. In other words, the film thickness of the resin layer listed in Table 2 means the distance from the outermost surface of the anodized film to the outermost surface of the resin layer.(2) Surface Observation
[0070] The surface (resin layer) of each sample was visually observed to check for the presence or absence of breakage (crack). The results are also listed in Table 2.(3) Cross-Sectional Observation
[0071] The longitudinal section of each sample was observed using the SEM. The SEM images obtained are collectively shown in FIGS. 3A and 3B (collectively referred to as “FIG. 3”). FIG. 3A shows the upper side near the treated surface, and FIG. 3B shows the lower side.«Evaluation»(1) Crack Resistance
[0072] As listed in Table 2, no cracks were observed on the surface of Sample 2, and it has been found that the crack resistance (heat resistance) is excellent. On the other hand, cracks were observed on the surfaces of the other samples. It is considered that such cracks are caused by thermal stress reflecting the difference in thermal expansion coefficient between the Al base material (metal) and the anodized film (ceramics). It is also considered that the anodized film of Sample 2 has a high porosity similar to that of Sample 1 and is highly flexible, so it is unlikely to crack.(2) Adhesion Properties
[0073] As can be seen from FIG. 3, in the case of Sample 2, polyimide penetrated into the anodized film, filling the main pores and also engaging with the sub-pores. This situation was hardly observed in the anodized films of the other samples. The reason why the main pores in Sample 2 were not filled with polyimide is considered to be that the polyimide broke / fell off when the test piece was cut.Third Example / Constant Voltage Electrolysis«Production of Samples»
[0074] The electrolytic step was performed by constant voltage DC energization on the test pieces composed of the aforementioned Al base material under the conditions listed in Table 3. The other processing conditions were the same as in First Example.«Measurements / Observations»
[0075] The test pieces (Samples 31 to 36) after anodization treatment for the samples were measured in the same manner as in First Example. The measurement results of porosity and opening diameter are also listed in Table 3. However, the field of view for Samples 31 to 33 was 2560 nm×1780 nm, and the field of view for Samples 34 to 36 was 1280 nm×890 nm.
[0076] SEM images obtained by observing the test piece surfaces (top surfaces) of the samples are shown in FIGS. 4A and 4B (both figures are collectively referred to as “FIG. 4”) as in First Example.«Evaluation»
[0077] As can be seen from Table 3 and FIG. 4, it has been found that when an electrolytic solution containing phosphoric acid is used, the higher the temperature (bath temperature) or the higher the applied voltage, the larger the porosity and opening diameter.
[0078] From the above, it has been confirmed that the anodized film of a unique form can be obtained by the present invention and the anodized film can exhibit high crack resistance at high temperatures, a high anchor effect for the upper layer, etc.TABLE 1Anodization treatment (Electrolytic step)EnergizationEvaluationVoltageAnodized filmTreatment bathCurrentafterTreatmentFilm OpeningSampleElectrolyteTemperaturedensity10 mintimethicknessdiameterPorosityNo.(Concentration)(°C)(mA / cm2)(V)(min)(μm)(μm)(%)1Phosphoric acid30301551291526(5%)A1Sulfuric acid1030571012177(20%)B1Oxalic acid30302210101399(5%)TABLE 2CoatingEvaluationAnodization treatment (Electrolytic step)Thickness Anodized filmTreatment bathCurrent Treatment of resinFilmCrack resistanceSampleElectrolyteTemperaturedensitytimelayerthickness(Presence or No.(Concentration)(°C)(mA / cm2)(min)(μm)(μm)absence of crack)2Phosphoric acid3030137310Absent(5%)A2Sulfuric acid1030 96310Present(20%)B2Oxalic acid3030107610Present(5%)TABLE 3EvaluationAnodization treatment (Electrolytic step)Anodized filmTreatment bathTreatment FilmOpeningSampleElectrolyteTemperatureVoltagetimethicknessdiameterPorosityNo.(Concentration)(°C)(V)(min)(μm)(μm)(%)31Phosphoric acid3050202953832(5%)10031423333150101782634Phosphoric acid1050201551535(5%)10011061236150214810
Claims
1. An aluminum-based member in which at least part of a surface of an aluminum base material is coated with an anodized film, whereinthe anodized film has main pores that extend in an approximately straight tube shape from the aluminum base material side and sub-pores that open on some of sidewalls of the main pores, andthe anodized film has a porosity of 18% to 65% when determined by observing a top surface of the anodized film.
2. The aluminum-based member according to claim 1, wherein the main pores have an opening diameter of 50 to 1000 nm.
3. The aluminum-based member according to claim 1, wherein the sub-pores are larger on an opening side than on a bottom side of the main pores.
4. The aluminum-based member according to claim 3, wherein one or more of the sub-pores are present in a surface region (depth 1 μm×width 10 μm) of an observed side surface.
5. The aluminum-based member according to claim 1, wherein at least some of the sub-pores penetrate the sidewalls of the main pores.
6. The aluminum-based member according to claim 1, wherein the anodized film has a film thickness of 0.1 to 20 μm.
7. The aluminum-based member according to claim 1, wherein the aluminum base material contains 98 mass % or more of Al relative to the aluminum base material as a whole.
8. The aluminum-based member according to claim 1, wherein the aluminum base material has an electric conductivity of 50% IACS or more.
9. The aluminum-based member according to claim 1, further comprising an upper layer that covers at least a portion of the anodized film.
10. The aluminum-based member according to claim 1, wherein at least a portion of the anodized film is coated with a resin.
11. The aluminum-based member according to claim 1, wherein it is an electrically-conductive member.
12. A method for producing an aluminum-based member, comprising an electrolytic step of energizing an aluminum base material that is in contact with an electrolytic solution containing phosphoric acid,wherein the aluminum-based member according to claim 1 is obtained.
13. The method for producing an aluminum-based member according to claim 12, wherein the electrolytic step is performed by keeping the electrolytic solution at 15 °C to 80 °C.
14. The method for producing an aluminum-based member according to claim 12, wherein the electrolytic step is performed by applying 30 to 250 V to the aluminum base material.