Method for producing positive electrode oxidation membrane and positive electrode oxidation membrane produced thereby
The method addresses the limitations of existing anodized membrane production by forming layers with varying solubilities and using heat treatments to produce large-area anodized membranes with uniform through-holes and enhanced chemical stability.
Patent Information
- Application Number
- US19/130154
- Authority / Receiving Office
- US · United States
- Patent Type
- Applications(United States)
- Current Assignee / Owner
- Priority Date
- 2022-11-16
- Filing Date
- 2023-11-16
- Publication Date
- 2026-11-19
AI Technical Summary
Existing methods for producing anodized porous alumina membranes face challenges in removing the barrier layer without enlarging pore diameters or being limited to small areas, and chemical dissolution techniques risk dissolving the pore walls.
A method involving multiple anodization processes to form layers with varying solubilities, using etching solutions to selectively dissolve layers with higher solubility, and heat treatments to stabilize the structure, enabling the production of through-hole membranes with controlled pore sizes and uniformity.
Enables the production of large-area anodized membranes with uniform through-holes and improved chemical stability, allowing for efficient and economical manufacturing of anodized membranes with controlled pore sizes and shapes.
Smart Images

Figure US20260366187A1-D00000_ABST
Abstract
Description
TECHNICAL FIELD
[0001] The present disclosure relates to a method for producing an anodized membrane and the anodized membrane produced by the method, and more particularly to a method for producing an anodized membrane, which includes forming anodized layers having different solubilities with respect to an etching solution, and removing one anodized layer having a relatively high solubility with respect to the etching solution, and the anodized membrane produced by the method.BACKGROUND
[0002] Aluminum is electrochemically anodized in an aqueous solution containing an electrolyte such as a sulfuric acid, an oxalic acid, or a phosphoric acid so that a thick anodized film is formed on a surface of the aluminum. In an anodized film, structures of a porous layer in which pores are grown at regular intervals from an outer surface toward an inner metal and a boundary layer, that is, a pore interval, a pore size, a thickness of the boundary layer, and the like are generally unaffected by a kind or temperature of the electrolyte, and are predominantly determined according to a voltage applied thereto.
[0003] A method for manufacturing an aluminum oxide film using such an electrochemical anodization have been disclosed in Patent Document by Alan W. Smith of Boeing company, 1974. In the method, aluminum is used as an anode in an electrochemical cell. In typical, an acidic solution made of an oxalic acid, a sulfuric acid, a phosphoric acid, or the like, is used as the electrolyte. Under most conditions, an amorphous oxide layer is produced. In 1995, Masuda and Fukuda found that a first anodization can produce pores aligned with time with respect to characteristic acid concentration, temperature and bias voltage, and developed an anodization method of two stages to produce aligned (hexagonal closed pack) porous aluminum oxide.
[0004] An anodized porous alumina has an alumina layer called a barrier layer formed on the bottom of a film. Thus, in a case in which the anodized porous alumina is used as a through-hole membrane, the barrier layer needs essentially to be removed.
[0005] As a method for removing the barrier layer, there are known a technique for physically cutting an alumina layer, such as Ar ion milling, and a technique for chemically dissolving the alumina layer. Since an apparatus capable of performing a penetration treatment without expanding a diameter of a pore is restricted in size, the technique such as the Ar ion milling is problematic for application to a large-area sample.
[0006] Meanwhile, the chemical dissolution technique is applicable to the large-area sample but is problematic in that since the pore is dissolved when the barrier layer is dissolved, the diameter of the pore diameter may be enlarged. That is, when the barrier layer is dissolved, an etching solution may flow into the pore so that a wall portion of the pore may be dissolved.
[0007] In general, the diameter of the pore of the porous alumina formed by the anodization is about ⅓ of a pore cycle. In a case in which a method for chemically treating a through-hole is used, it is difficult to form a through-hole membrane having a pore that are not more than ⅓ of the pore cycle.
[0008] In a case in which an anodized alumina membrane in which the barrier layer has significantly higher solubility than another alumina layer may be produced, the chemical dissolution technique may be used to produce a through-hole membrane having a small pore diameter. However, a method for producing such an anodized porous alumina membrane has not been known.SUMMARY OF THE PRESENT DISCLOSURETechnical Problem
[0009] The present disclosure was made for the purpose of solving the above matters in the conventional technology, and the present disclosure is for the purpose of a method for producing a through-hole type anodized membrane, which is capable of removing a barrier layer using a difference in solubility.
[0010] Further, the present disclosure is for the purpose of the through-hole type anodized membrane produced by the method of the present disclosure.Technical Solution
[0011] The present disclosure was made to solve the above-mentioned matters, and the present disclosure provides a method for producing an anodized membrane, the method comprising:
[0012] (a) preparing an aluminum substrate;
[0013] (b) performing a surface treatment on the aluminum substrate;
[0014] (c) forming a first anodized layer on one surface of the aluminum substrate by a first anodization process;
[0015] (d) removing the first anodized layer made in step (c) with a first etching solution to form a seed layer;
[0016] (e) forming a second anodized layer from the seed layer of the aluminum substrate by a second anodization process;
[0017] (f) performing a first heat treatment on the aluminum substrate on which the second anodized layer is formed;
[0018] (g) forming a third anodized layer below the second anodized layer of the aluminum substrate by a third anodization process; and
[0019] (h) immersing the aluminum substrate in a second etching solution to remove the third anodized layer.
[0020] In the method for producing the anodized membrane according to the present disclosure, the first anodization process in the step (c) includes anodizing the aluminum substrate using any one or more selected from a group consisting of a sulfuric acid, an oxalic acid, and a phosphoric acid to form the first anodized layer.
[0021] In the method for producing the anodized membrane according to the present disclosure, a thickness of the first anodized layer is 20 micrometers or more. In the method for producing the anodized membrane according to the present disclosure, a convex portion is formed in the first anodized layer and to be used as a seed layer in a subsequent process. Thus, the thickness is preferably 20 micrometers or more.
[0022] In the method for producing the anodized membrane according to the present disclosure, a solubility of the third anodized layer with respect to the etching solution is higher than a solubility of the second anodized layer with respect to the etching solution. The method for producing the anodized membrane according to the present disclosure uses a difference in the solubilities of the anodized layers with respect to the etching solution such that the third anodized layer is preferentially dissolved by setting the solubility of the third anodized layer with respect to the second etching solution close to that of an aluminum base material, and the second anodized layer and the aluminum base material are separated from each other to produce the anodized membrane including through-holes formed in the second anodized layer.
[0023] In the method for producing the anodized membrane according to the present disclosure, the step (f)of performing the first heat treatment on the aluminum substrate on which the second anodized layer is formed is performed at a temperature of 800° C. or higher.
[0024] In the method for producing the anodized membrane according to the present disclosure, crystal structures of minute regions of the second anodized layer, which was subjected to the heat treatment described above, are changed by desorption of adsorbed water and hydrated water so that the second anodized layer is chemically stabilized. Therefore, the resistance of the first anodized layer to an electrolytic solution and the like is improved by the first heat treatment. Further, the higher the temperature of the first heat treatment and the longer the time required for the first heat treatment, the higher a ratio of crystalline alumina. Accordingly, the effect is increased. Further, the anodized membrane according to the present disclosure is formed by making the anodized layers contact with each other having different solubilities respect with each other. Thus, in a site where the anodized membranes having different solubilities are in contact with each other, the anodized membrane having a relatively high solubility may not be formed uniformly. As a result, when the anodized membrane is dissolved with the second etching solution, a structure thereof may become uneven. By making the distribution of anions uniform through the first heat treatment, the flatness of the resultantly-formed anodized membrane may be improved.
[0025] In the method for producing the anodized membrane according to the present disclosure, the step (g) of forming the third anodized layer is performed by using any one or more selected from a group consisting of a sulfuric acid, an oxalic acid, and a phosphoric acid, and applying a pulse voltage for anodization.
[0026] In the method for producing the anodized membrane according to the present disclosure, a thickness of the third anodized layer is 2 micrometers or less.
[0027] The method for producing the anodized membrane according to the present disclosure includes a third anodization process of forming a second anodized layer to be etched away in a subsequent operation. The third anodization process includes applying a pulse voltage to stably form the second anodized layer in a wide range while reducing the thickness of the second anodized layer.
[0028] Anodizing using a pulse current is a kind of cycle plating in which a current waveform is cyclically changed between an anode and a cathode, that is, a constant current (plating) and a reverse current (reverse), in a repetitive manner for a certain period of time. A waveform of the pulse being most widely used is a square pulse waveform, which is mainly used in a radio frequency band.
[0029] In the method for producing the anodized membrane according to the present disclosure, the polarity is alternately changed in a certain period to prevent a concentration of anions acting to dissolve an oxidation layer from being concentrated at the anode, prevent the application of the overvoltage, suppress the dissolution of the oxidation layer, and form a firm oxidation layer. In particular, in the case of producing a large-area anodized membrane, a high voltage needs to be applied. However, since the high voltage thus applied may be concentrated only at a certain portion, the voltage may be preferably applied in the form of a pulse, more preferably, in a square pulse waveform.
[0030] In the method for producing the anodized membrane according to the present disclosure, in the step (e), the first anodized layer is formed by the first anodization process of immersing the aluminum substrate in an oxalic acid solution of 0.2 M to 1.0 M, and performing anodization at an application voltage of 40 volt (V) and a maximum current limit of 10 ampere (A) for a time period of 1 hour to 10 hours while maintaining a solution temperature in a range of 20 degree Celsius (° C.) to 30° C.
[0031] In the method for producing the anodized membrane according to the present disclosure, in the third anodization process, the third anodized layer is formed by the second anodization process of immersing the aluminum substrate in an sulfuric acid solution of 1.0M to 20.0M, and performing the anodization by applying a pulse voltage in 30 to 50 cycles, one cycle including applying a voltage of 50V to 60V for 2 seconds to 6 seconds and subsequently applying a voltage of 35V to 45V for 2 seconds to 6 seconds while maintaining the solution temperature in a range of 0° C. to 30° C.
[0032] In the method for producing the anodized membrane according to the present disclosure, in the step Vi), the third anodized layer is formed by the third anodization process of immersing the aluminum substrate in the sulfuric acid solution of 1.0 M to 20.0 M, and applying a pulse voltage in 30 to 50 cycles, one cycle including applying a voltage of 50 V to 60 V for 2 seconds to 6 seconds and subsequently applying a voltage of 35 V to 45 V for 2 seconds to 6 seconds while maintaining the solution temperature in a range of 0° C. to 30° C.
[0033] In the method for producing the anodized membrane according to the present disclosure, the first etching solution in the step (d) includes one or more selected from a group consisting of a nitric acid and a phosphoric acid.
[0034] In the method for producing the anodized membrane according to the present disclosure, the second etching solution in the step (h) includes one or more selected from a group consisting of a chromic acid, a nitric acid, and a phosphoric acid. In the method for producing the anodized membrane according to the present disclosure, the second etching solution in the step (h) includes a chromic acid.
[0035] In the method for producing the anodized membrane according to the present disclosure, the step (b) of performing the surface treatment on the aluminum substrate is performed by electropolishing or chemical polishing. In the method for producing the anodized membrane according to the present disclosure, an electrolytic treatment may be performed with a mixed solution of ethanol and perchloric acid (for example, a ratio of ethanol to perchloric acid=4:1) to remove a film formed on the surface of the aluminum substrate in advance and flatten the surface if necessary. The electrolytic treatment may be performed for 3 minutes under conditions of a temperature of, for example, 10° C. or less, and 1,000A / m2.
[0036] In the method for producing the anodized membrane according to the present disclosure, the steps (e) to (h) are further repeatedly performed after the step (h). In the method for producing the anodized membrane according to the present disclosure, the third anodized layer is removed in the step (h) so that the anodized membrane including through-holes formed in the second anodized layer and the aluminum substrate are separated from each other.
[0037] The aluminum substrate separated at this time is in the state in which the seed layer is formed after the formation of the first anodized layer. Thus, the first anodized layer can be additionally formed. The steps (e) to (h) may be performed based the seed layer to form the second anodized layer and the third anodized layer, and remove the third anodized layer having the relatively high solubility with respect to the etching solution, thereby further producing the anodized membrane including through-holes formed in the second anodized layer. Further, the steps may be repeatedly performed to form a plurality of anodized membranes based on one aluminum substrate.
[0038] According to the present disclosure, unlike in the conventional technology in which one aluminum substrate is used to produce only one anodized membrane, the plurality of anodized membranes may be produced using one aluminum substrate. This is economical and makes it possible to continuously maintain the seed layer formed in the aluminum substrate, thus increasing a degree of arrangement of the pores.
[0039] The method for producing the anodized membrane according to the present disclosure may further include performing a second heat treatment after the step (g). In the method for producing the anodized membrane according to the present disclosure, the second heat treatment is performed at a temperature of 1,000° C. or higher. In the method for producing the anodized membrane according to the present disclosure, the anodized layer, that is, the porous material, may be crystallized by the second heat treatment. This makes it possible to improve chemical properties, that is, chemical stability, such as heat resistance, acid resistance, alkaline resistance, high-temperature resistance, and the like, and expand an application range of the porous material thus obtained.
[0040] Further, the present disclosure provides the anodized membrane produced by the method according to the present disclosure.
[0041] The anodized membrane produced according to the present disclosure may have a large area and the length of one side is 20 centimeter (cm) or more.
[0042] In the anodized membrane produced according to the present disclosure, each through-hole is formed to extend from a first surface to a second surface, and one end of each through-hole in the first surface has a tapered shape.Advantageous Effects
[0043] According to the method for producing an anodized membrane according to the present disclosure, anodized layers having different solubilities may be produced. One anodized layer having a relatively high solubility may be first dissolved by an etching solution. The anodized membrane produced by the method according to the present disclosure may have through-holes formed to extend from a first surface to a second surface.BRIEF DESCRIPTION OF THE DRAWINGS
[0044] FIG. 1 illustrates anodized membranes produced in Example of the present disclosure and Comparative Example.
[0045] FIGS. 2 and 3 illustrate photographs obtained by measuring the anodized membrane produced according to Example of the present disclosure by a scanning electrochemical microscopy (SEM).
[0046] FIGS. 4 and 5 illustrate photographs obtained by measuring the anodized membrane produced in Comparative Example of the present disclosure by the SEM.
[0047] FIGS. 6A to 6C illustrate photographs obtained by measuring a first surface and a second surface of the anodized membrane produced according to Examples of the present disclosure by SEM.DETAILED DESCRIPTION
[0048] Hereinafter, Examples of the present disclosure will be described in more detail. However, the present disclosure is not limited by the following Examples.Example 1
[0049] An aluminum plate having a purity of 99.999 percent(%) and a size of 100 millimeter (mm)×150 mm was prepared. Electropolishing was performed on the aluminum plate in a mixed solution of perchloric ethanol to clean a surface of the aluminum plate.
[0050] A first anodization process of forming a seed layer was performed for 60 minutes with an oxalic acid of 0.5 mol / liter at a solution temperature of 30 degree Celsius (° C.), an application voltage of 40 volt (V) and a maximum current limit of 10 amperes (A) to form a first anodized layer.
[0051] Subsequently, a mixed solution of 1.8 weight (wt)% of chromic acid and 6 wt% of phosphoric acid was used as an etching solution. The aluminum substrate was immersed in the mixed solution at a solution temperature of 60° C. for 3 hours to completely remove the first anodized layer and form a regular seed arrangement.
[0052] Subsequently, the aluminum substrate was washed with distilled water and a second anodization process was performed for 60 minutes with the oxalic acid of 0.5 M at the solution temperature of 30° C., the application voltage of 40 V and the maximum current limit of 10A to form a second anodized layer. Thereafter, the aluminum substrate on which the second anodized layer is formed was subjected to a first heat treatment at a temperature of 800° C. for 5 hours.
[0053] After the aluminum plate on which a second layer of an anodized membrane or positive electrode oxidation membrane is formed was washed with the distilled water, a pulse anodization was performed by applying a pulse voltage in 40 cycles, one cycle including applying 55 V for 3 seconds and 40 V for 5 seconds with the sulfuric acid of 12 M at the solution temperature of 0° C., so that a third anodized layer having a relatively high solubility with respect to the etching solution was formed below the second anodized layer.
[0054] The aluminum substrate thus obtained was washed with the distilled water, and subsequently, the aluminum substrate on which the third anodized layer and the first anodized layer is formed was subjected to a second heat treatment at 1,000° C. for 5 hours.
[0055] Subsequently, a sample was immersed in 6 wt% of phosphoric acid solution as an etching solution for 10 minutes at the solution temperature of 40° C. to remove the third anodized layer having the relatively high solubility.
[0056] After the etching, the aluminum substrate was washed with the distilled water and was dried to obtain an separated anodized membrane including through-holes formed in the second anodized layer.Example 2
[0057] Chemical polishing was performed on an aluminum plate having a purity of 99.5% and a size of 200 mm×150 mm to clean a surface of the aluminum plate.
[0058] A first anodization process of forming a seed layer was performed for 90 minutes with an oxalic acid of 0.5 M at a solution temperature of 27° C., an application voltage of 60 V and a maximum current limit of 20 A to form a first anodized layer.
[0059] Subsequently, a mixed solution of 1.8 wt% of chromic acid and 6 wt% of phosphoric acid was used as an etching solution. The aluminum substrate was immersed in the mixed solution at the solution temperature of 60° C. for 3 hours to completely remove the first anodized layer and form a regular seed arrangement.
[0060] Subsequently, the aluminum substrate was washed with distilled water and a second anodization process was performed for 90 minutes with the oxalic acid of 0.5 M at the solution temperature of 27° C., the application voltage of 60 V and the maximum current limit of 20 A to form a second anodized layer. Thereafter, the aluminum substrate on which the second anodized layer is formed was subjected to a first heat treatment at a temperature of 800° C. for 3 hours.
[0061] After the aluminum plate on which the second anodized layer is formed was washed with the distilled water, a pulse anodization was performed by applying a pulse voltage in 50 cycles, one cycle including applying 55 V for 3 seconds and 40 V for 5 seconds with the sulfuric acid of 12 M at the solution temperature of 0° C., so that a third anodized layer having a relatively high solubility with respect to the etching solution was formed below the second anodized layer.
[0062] The aluminum substrate thus obtained was washed with the distilled water and was dried in an oven kept at 45° C. for 20 minutes, and subsequently, the aluminum substrate on which the third anodized layer is formed was subjected to a second heat treatment at 1,000° C. for 3 hours.
[0063] Subsequently, a sample was immersed in 6 wt% of phosphoric acid solution as an etching solution for 10 minutes at the solution temperature of 40° C. to remove the third anodized layer having the relatively high solubility, so that the aluminum substrate and an anodized membrane including the second anodized layer were separated from each other.
[0064] The membrane including the second anodized layer thus separated was washed with the distilled water and was dried to obtain an anodized membrane including through-holes.Example 3
[0065] An aluminum plate having a purity of 99.5% and a size of 100 mm×150 mm was prepared, and chemical polishing was performed on the aluminum plate to clean a surface of the aluminum plate.
[0066] A first anodization process was performed for 90 minutes with an oxalic acid of 0.3 M at a solution temperature of 2° C., an application voltage of 40 V and a maximum current limit of 3 A to form a first anodized layer.
[0067] Subsequently, a mixed solution of 1.8 wt% of chromic acid and 6 wt% of phosphoric acid was used as an etching solution. The aluminum substrate was immersed in the mixed solution at the solution temperature of 40° C. for 24 hours to completely remove the first anodized layer and form a regular seed arrangement.
[0068] Subsequently, the aluminum substrate was washed with distilled water and a second anodization process was performed for 90 minutes with the oxalic acid of 0.3 M at the solution temperature of 2° C., the application voltage of 40 V and the maximum current limit of 3 A to form a second anodized layer. Thereafter, the aluminum substrate on which the second anodized layer is formed was subjected to a first heat treatment at a temperature of 850° C. for 3 hours.
[0069] After a sample thus formed was washed with the distilled water, the sample was immersed for 30 minutes in a mixed etching solution of 1.8 wt% of chromic acid and 6 wt% of phosphoric acid at the solution temperature of 40° C. to widen a size of each pore and reduce a thickness of a barrier layer.
[0070] After the aluminum plate is washed with the distilled water, a pulse anodization was performed by applying a pulse voltage in 30 cycles for 4 minutes, one cycle including applying 45 V at the maximum current limit of 3 A for 3 seconds and 30 V at the maximum current limit of 3 A for 5 seconds (for a total of 8 seconds) with the sulfuric acid of 12 M at the solution temperature of 0° C., so that a third anodized layer having a relatively high solubility with respect to the etching solution compared to the second anodized layer was formed below the second anodized layer.
[0071] The aluminum substrate thus obtained was washed with the distilled water and was dried in an oven kept at 45° C. for 20 minutes, and subsequently, the aluminum substrate on which the third anodized layer is formed was subjected to a second heat treatment at 1,100° C. for 3 hours.
[0072] Subsequently, a sample was immersed in 6 wt% of phosphoric acid solution as an etching solution for 10 minutes at the solution temperature of 40° C. to remove the third anodized layer having the relatively high solubility, so that the aluminum substrate and a membrane including the second anodized layer were separated from each other.
[0073] The membrane thus separated was washed with the distilled water and was dried to obtain an anodized membrane including through-holes formed in the second anodizied layer.Example 4
[0074] The aluminum substrate separated in the Example 2 above includes the seed layer obtained by forming and removing the first anodized layer. Thus, the anodized membrane was produced again using the aluminum substrate.
[0075] The aluminum substrate thus separated was washed with the distilled water and a second anodization process was performed for 90 minutes with the oxalic acid of 0.5 M at the solution temperature of 27° C., the application voltage of 60 V and the maximum current limit of 20 A to form a second—1st anodized layer. Thereafter, the aluminum substrate on which the second anodized layer is formed was subjected to a first—1st heat treatment at a temperature of 800° C. for 3 hours.
[0076] After the aluminum substrate on which the second anodized layer is formed is washed with the distilled water, a pulse anodization was performed by applying a pulse voltage in 50 cycles, one cycle including applying 55 V for 3 seconds and 40 V for 5 seconds with the sulfuric acid of 12 M at the solution temperature of 0° C., so that a third anodized layer having a relatively high solubility with respect to the etching solution was formed below the second anodized layer.
[0077] The aluminum substrate thus obtained was washed with the distilled water and was dried in an oven kept at 45° C. for 20 minutes, and subsequently, the aluminum substrate on which the third anodized layer is formed was subjected to a second—2nd heat treatment at 1,000° C. for 3 hours.
[0078] Subsequently, a sample was immersed in 6 wt% of phosphoric acid solution as an etching solution for 10 minutes at the solution temperature of 40° C. to remove the third anodized layer having the relatively high solubility, so that the aluminum substrate and an anodized membrane including the second anodized layer were separated from each other.
[0079] The membrane including the second anodized layer thus separated was washed with the distilled water and was dried to obtain an anodized membrane including through-holes.Comparative Example
[0080] A anodized membrane including through-holes was obtained in the same manner as in Example 3 above except that the first heat treatment was not performed after the formation of the first anodized layer, the anodization process was performed for 4 minutes by applying a constant voltage rather than the pulse voltage with the sulfuric acid of 12 M at the solution temperature of 0° C. and the current limit of 3 A to form the third anodized layer, and the second heat treatment was not performed after the formation of the third anodized layer formation.<Experimental Example>Measurement by Membrane Photograph
[0081] FIG. 1 illustrates AAO membranes produced in Example 3 and Comparative Examples above.
[0082] It was found from FIG. 1 that, in the case in which the pulse voltage is applied as in Example 3, the membrane is produced evenly over a large area of 20 cm×20 cm, while in the case in which the constant voltage is applied as in Comparative Example, a high voltage is applied to form the membrane over the large area so that the membrane at a portion connected to an electrode may be deteriorated and broken due to such an overvoltage.<Experimental Example>Measurement by SEM Analysis
[0083] The anodized membranes produced in Example 3 and Comparative Example above were measured by SEM analysis. SEM measurement results of Example 3 are illustrated in FIGS. 2 and 3, and SEM measurement results of Comparative Example are illustrated in FIGS. 4 and 5.
[0084] It was found from FIGS. 2 and 4 that Example and Comparative Example are similar to each other in terms of a pore size and pore uniformity, while in Example in which the pulse voltage is applied, the membrane is formed uniformly over the large area of 20 cm×20 cm and the pore uniformity is further improved by the first heat treatment and the second heat treatment. It was found from results obtained by measuring the sides as illustrated in FIGS. 3 and 5 that, even if the anodization process is performed for 4 minutes in both Example and Comparative Example, the thickness of the third anodized layer is smaller in Example 3 in which the pulse voltage is applied than Comparative Example in which the constant voltage is applied.
[0085] Further, it was found from FIGS. 3 and 5 that in Example of the present disclosure in which the pulse voltage is applied, a boundary between the second anodized layer and the third anodized layer is uniform.
[0086] In addition, it was found from FIGS. 6A to 6C that the anodized membrane produced in Example of the present disclosure includes through-holes extending a first surface to a second surface. As illustrated in FIG. 6A, it was found that an end of each through-hole constituting the first surface has a tapered shape.CROSS-REFERENCE TO RELATED APPLICATION
[0087] This application claims the benefits of Korean Patent Applications No. 10-2022-0153657 filed with Korean Patent Office on Nov. 16, 2022; and No. 10-2022-0153663 filed with Korean Patent Office on Nov. 16, 2022; and No. 10-2022-0153668 filed with Korean Patent Office on Nov. 16, 2022, under Article 119 (a) (35 U.S.C. § 119 (a)) of U.S. Patent Act, the entire contents of which are incorporated herein by references. Further, this application claims the same priorities with respect to countries other than the United States, the entire contents of which are incorporated herein by references.
Claims
1-16. (canceled)17. A method for producing an anodized membrane, the method comprising:(a) a step of preparing an aluminum substrate;(b) a step of performing a surface treatment on the aluminum substrate;(c) a step of forming a first anodized layer on one surface of the aluminum substrate by a first anodization process;(d) a step of removing the first anodized layer made in step (c) with a first etching solution to forming a seed layer;(e) a step of forming a second anodized layer from the seed layer of the aluminum substrate by a second anodization process;(f) a step of performing a first heat treatment on the aluminum substrate on which the second anodized layer is formed;(g) a step of forming a third anodized layer below the second anodized layer of the aluminum substrate by a third anodization process; and(h) a step of immersing the aluminum substrate in a second etching solution to remove the third anodized layer.
18. The method of claim 17, wherein the first anodization process in the step (c) includes anodizing the aluminum substrate using any one or more selected from a group consisting of a sulfuric acid, an oxalic acid, and a phosphoric acid to form the first anodized layer.
19. The method of claim 17, wherein a thickness of the first anodized layer is 20 micrometers or more.
20. The method of claim 17, wherein a solubility of the third anodized layer with respect to the second etching solution is higher than a solubility of the second anodized layer with respect to the second etching solution.
21. The method of claim 17, wherein the step (f) of performing the first heat treatment on the aluminum substrate on which the second anodized layer is formed is performed at a temperature of 800° C. or higher.
22. The method of claim 17, wherein the step (g) of forming the third anodized layer is performed by using any one or more selected from a group consisting of a sulfuric acid, an oxalic acid, and a phosphoric acid, and applying a pulse voltage for anodization.
23. The method of claim 17, wherein a thickness of the third anodized layer is 2 micrometers or less.
24. The method of claim 17, wherein the step (e) of forming the second anodized layer includes:immersing the aluminum substrate in an oxalic acid solution of 0.2 M to 1.0 M; andperforming the second anodization process at an application voltage of 40 V and a maximum current limit of 10 A to 20 A for a time period of 1 hour to 10 hours while maintaining a solution temperature in a range of 20° C. to 30° C.
25. The method of claim 17, wherein the step (g) of forming the third anodized layer includes:immersing the aluminum substrate a sulfuric acid solution of 1.0 M to 20.0 M; andperforming the third anodization process by applying a pulse voltage in 30 to 50 cycles, one cycle including applying a voltage of 50 V to 60 V for 2 seconds to 6 seconds and subsequently applying a voltage of 35 V to 45 V for 2 seconds to 6 seconds while maintaining a solution temperature in a range of 0° C. and 30° C.
26. The method of claim 17, wherein the first etching solution in the step (d) includes one or more selected from a group consisting of a nitric acid and a phosphoric acid.
27. The method of claim 17, wherein the second etching solution in the step (h) includes one or more selected from a group consisting of a chromic acid, a nitric acid, and a phosphoric acid.
28. The method of claim 17, wherein the step (b) of performing the surface treatment on the aluminum substrate is performed by electropolishing or chemical polishing.
29. The method of claim 17, wherein the step (h) of immersing the aluminum substrate in the second etching solution to remove the third anodized layer includes:separating the anodized membrane including the second anodized layer from the aluminum substrate including the first anodized layer; andrepeatedly performing the steps (e) to (h) on the aluminum substrate including the first anodized layer separated in the separation step.
30. The method of claim 17, further comprising: performing a second heat treatment after the step (g).
31. The method of claim 30, wherein the second heat treatment is performed at a temperature of 1,000° C. or more.
32. An anodized membrane produced by the method of claim 17, wherein at least of one surface of the anodized membrane has a tapered shape.