Reverse contact photovoltaic cell manufacturing method

VN10062323BActive Publication Date: 2026-10-15LONGI SOLAR TECHNOLOGY (TAIZHOU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
VN1202401842
Authority / Receiving Office
VN · VN
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-09-30
Filing Date
2022-05-11
Publication Date
2026-10-15
Estimated Expiration
2042-05-11

AI Technical Summary

Technical Problem

The existing preparation methods for back contact cells are complicated and the steps are cumbersome, making it difficult to prepare high-efficiency solar cells.

Method used

A back contact battery manufacturing method is adopted, by forming staggered doping regions and doping layers on the surface of the substrate, and using laser irradiation to form an oxide mask layer, simplifying the process steps and reducing the removal process of the mask layer. Improve electrical conductivity and photoelectric conversion efficiency.

Benefits of technology

The manufacturing process of the back-contact battery is simplified, the photoelectric conversion efficiency and the conductive performance of the battery are improved, the contact area between the metal electrode and the doped layer is reduced, the carrier recombination rate is reduced, and the open circuit voltage is increased.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure VN1202401842_0
    Figure VN1202401842_0
Patent Text Reader

Abstract

The invention relates to a method for producing reverse-contact cells, relating to the field of photovoltaic technology, and used to simplify the manufacturing process. The manufacturing method includes: providing a substrate; sequentially forming the first separating passivation layer and the first doping layer on the first surface of the substrate; forming the first barrier layer only on the surface of the first doping layer located within the first doping zone; removing the first doping layer and the first separating passivation layer located within the second and third doping zones; sequentially forming the second separating passivation layer and the second doping layer on the first barrier layer, the second doping zone, and the third doping zone simultaneously, wherein the conductive type of the second doping layer is opposite to the conductive type of the first doping layer; forming the second barrier layer only on the surface of the second doping layer located within the second doping zone;Remove the second doping layer and the second separating passivation layer located above the first barrier layer and the third region, while maintaining only the second separating passivation layer and the second doping layer within the second doping region; and form the first electrode on the first doping layer, and form the second electrode on the second doping layer.
Need to check novelty before this filing date? Find Prior Art

Description

Method for manufacturing a back contact battery

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This disclosure claims priority to a Chinese patent application filed with the Patent Office of China on September 30, 2021, with application number 202111165394.2 and titled “A Method for Manufacturing a Back-Contact Battery,” the entire contents of which are incorporated by reference into this disclosure. Technical Field

[0003] The present invention relates to the field of photovoltaic technology, and in particular to a method for manufacturing a back-contact battery. Background Art

[0004] Back-contact cells are cells with both the emitter and metal contacts on the back of the cell, leaving the front unobstructed by metal electrodes. Compared to cells with obstructed fronts, back-contact cells offer higher short-circuit current and photoelectric conversion efficiency, and are currently one of the technological advancements in achieving high-efficiency crystalline silicon cells.

[0005] The existing method for preparing back-contact solar cells is relatively complicated and involves many steps. Therefore, a method for preparing solar cells that is simple and ensures high efficiency is needed.

[0006] Summary of the Invention

[0007] The object of the present invention is to provide a method for manufacturing a back-contact battery to simplify the manufacturing process of the back-contact battery.

[0008] In a first aspect, the present invention provides a method for manufacturing a back-contact battery, comprising:

[0009] A substrate is provided, wherein the substrate has a first surface and a second surface opposite to each other, wherein the first surface has first doped regions and second doped regions arranged alternately, and a third region for spacing the first doped regions and the second doped regions;

[0010] forming a first interface passivation layer and a first doping layer in sequence on the first surface of the substrate;

[0011] forming a first mask layer only on the surface of the first doping layer located in the first doping region;

[0012] removing the first doping layer and the first interface passivation layer located on the second doping region and the third region;

[0013] forming a second interface passivation layer and a second doping layer simultaneously and sequentially on the first mask layer, the second doping region and the third region, wherein the second doping layer has a conductivity type opposite to that of the first doping layer;

[0014] forming a second mask layer only on the surface of the second doping layer located in the second doping region;

[0015] removing the second doping layer and the second interface passivation layer located on the first mask layer and the third region, and retaining only the second interface passivation layer and the second doping layer located in the second doping region;

[0016] A first electrode is formed on the first doping layer, and a second electrode is formed on the second doping layer.

[0017] When the above technical solution is adopted, during the patterning process of the first doping layer and the second doping layer, a mask layer can be formed only in the required area, avoiding the formation of unnecessary mask layers in other areas, and reducing the steps of removing the mask layers in unnecessary areas. In addition, the patterning of the second doping layer (i.e., the process of removing the second doping layer in the area outside the second mask layer) and the formation of the third area are completed in the same step, which simplifies the steps. In addition, when making the second doping layer and patterning the second doping layer, the first mask layer is always retained on the first doping layer. Therefore, during the patterning process of the second doping layer, due to the protective effect of the first mask layer on the first doping layer, the damage to the first doping layer is reduced, thereby ensuring the conductive performance of the first doping layer.

[0018] In some possible implementations, the first mask layer is a first oxide mask layer; and / or the second mask layer is a second oxide mask layer. Both the first and second mask layers are oxide mask layers, which can be formed directly on the first and second doped layers by oxidation. Compared to other separately prepared mask layers, such as printed masks, oxide mask layers have a high degree of cleanliness, do not introduce other elements, and do not contaminate or affect the first and second doped layers. Oxide masks are easy to clean.

[0019] In some possible implementations, the first oxide mask layer is formed by laser irradiation oxidation only on the surface of the first doped layer located in the first doped region in an oxygen-containing atmosphere; and / or the second oxide mask layer is formed by laser irradiation oxidation only on the surface of the second doped layer located in the second doped region in an oxygen-containing atmosphere. In this configuration, the oxide mask layer is formed directly on the first doped layer and the second doped layer by laser irradiation, resulting in high-precision formation of the oxide mask layer. Compared to mask layers formed by external thermal oxidation or PECVD methods, the laser irradiation process generates less heat, thereby reducing damage to the first doped layer and the second doped layer.

[0020] In some possible implementations, the gas in the oxygen-containing atmosphere is one or more of oxygen, ozone, air, CO2, and N2O. In this oxygen-containing atmosphere, laser irradiation allows the first doped layer and the second doped layer to undergo an oxidation reaction with the gas, forming an oxide mask layer on the surface.

[0021] In some possible implementations, an alkaline solution is used to remove the second doping layer and the second interface passivation layer located on the first mask layer and the third region, and the same alkaline solution is used to continue to form a velvet structure simultaneously in the third region and the second surface of the first surface. With this arrangement, multiple processes of patterning the second doping layer, patterning the third region, and texturing the second surface of the substrate can be completed simultaneously in the same step using the same alkaline solution. The number of process steps is greatly reduced. The velvet structure of the third region increases the light trapping level on the back of the back contact battery and improves power generation. The second surface texturing process is placed after the formation of the first doping layer and the second doping layer, ensuring the integrity of the velvet structure of the second surface and its light trapping performance.

[0022] In some possible implementations, at 70°C to 90°C, an alkaline solution of KOH, NaOH or tetramethylammonium hydroxide with a mass percentage of 1 wt% to 5 wt% is used to remove the second doping layer and the second interface passivation layer located on the first mask layer and the third region, and the same alkaline solution is used to continue to form a velvet structure on the third region of the first surface and the second surface at the same time.

[0023] In some possible implementations, forming a first electrode on the first doped layer and forming a second electrode on the second doped layer specifically includes the following steps:

[0024] removing the first mask layer located on the first doped layer and the second mask layer located on the second doped layer;

[0025] forming a first surface passivation layer on the first doping layer, the second doping layer and the third region simultaneously;

[0026] A first electrode is formed on the first surface passivation layer of the first doping layer, and a second electrode is formed on the first surface passivation layer of the second doping layer. The first electrode is in electrical contact with the first doping layer, and the second electrode is in electrical contact with the second doping layer.

[0027] When the above technical solution is adopted, after the patterning of the first doping layer and the second doping layer and the formation of the third region are completed, the first mask layer and the second mask layer can be removed to improve the conductive contact performance between the first doping layer and the first electrode, and between the second doping layer and the second electrode. In addition, the first surface passivation layer can perform surface passivation on the back contact battery, passivate the dangling bonds in the first doping layer, the second doping layer and the third region, reduce the carrier recombination velocity on the first surface, and improve the photoelectric conversion efficiency. The first electrode and the second electrode are electrically contacted with the first doping layer and the second doping layer through the first opening and the second opening, respectively, to form a local ohmic contact between the metal and the semiconductor, reducing the contact area between the metal electrode and the first doping layer and the second doping layer, reducing the contact resistance, further reducing the carrier recombination velocity at the electrode surface, and improving the open circuit voltage.

[0028] In some possible implementations, the first mask layer and the second mask layer are removed using an etching solution containing fluorine. The etching solution containing fluorine can more easily remove the mask layer, especially the oxide mask layer; and / or

[0029] The step of simultaneously forming a first surface passivation layer on the first doped layer, the second doped layer, and the third region further includes forming a second surface passivation layer on the second surface. This arrangement allows the second surface passivation layer to be formed in the same step as the first surface passivation layer, simplifying the process. Furthermore, the second surface passivation layer has the effects of reducing incident light reflection and passivating the layer.

[0030] In some possible implementations, the first doping layer and the second doping layer are formed by an in-situ doping method or an ex-situ doping method.

[0031] In some possible implementations, before forming the first electrode on the first doped layer and the second electrode on the second doped layer, the process further includes: performing a heat treatment process to crystallize at least a portion of the first doped layer and / or the second doped layer. This configuration improves the electrical conductivity of the first doped layer and / or the second doped layer, and the heat treatment makes the first and second interface passivation layers more conducive to carrier selectivity and transport. Heating can also allow the doping elements to enter the first and second interface passivation layers and the substrate, thereby reducing transmission resistance.

[0032] The above description is only an overview of the technical solution of the present disclosure. In order to more clearly understand the technical means of the present disclosure, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present disclosure more obvious and easy to understand, the specific implementation methods of the present disclosure are listed below. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to more clearly illustrate the technical solutions in the embodiments of the present disclosure or related technologies, the following is a brief introduction to the drawings required for use in the embodiments or related technical descriptions. Obviously, the drawings described below are some embodiments of the present disclosure. For ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.

[0034] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0035] FIG1 is a schematic structural diagram of a back-contact battery provided by an embodiment of the present invention;

[0036] 2 to 10 are schematic diagrams of various stages of a back contact battery manufacturing process according to an embodiment of the present invention;

[0037] FIG11 is a schematic diagram of the laser irradiation principle used in a method for manufacturing a back-contact cell provided by an embodiment of the present invention;

[0038] FIG12 is a schematic flow chart of a method for manufacturing a back-contact battery provided in an embodiment of the present invention.

[0039] Reference numerals:

[0040] 10-substrate, 101-first doping region,

[0041] 102 - second doping region, 103 - third region,

[0042] 11-first doping layer, 12-second doping layer,

[0043] 13-first surface passivation layer, 131-first opening,

[0044] 132-second opening, 14-first interface passivation layer,

[0045] 15-second interface passivation layer, 16-first mask layer,

[0046] 17-second mask layer, 18-second surface passivation layer,

[0047] 20-first electrode, 21-second electrode,

[0048] 30-first electrode, 301-air inlet,

[0049] 302-Exhaust port Specific embodiments

[0050] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention more clearly understood, the present invention is further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0051] It should be noted that when an element is referred to as being “fixed on” or “disposed on” another element, it may be directly on the other element or indirectly on the other element. When an element is referred to as being “connected to” another element, it may be directly connected to the other element or indirectly connected to the other element.

[0052] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be understood to indicate or imply relative importance or implicitly specify the number of the technical features indicated. Thus, a feature specified as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, "plurality" means two or more, unless otherwise specifically defined. "Several" means one or more, unless otherwise specifically defined.

[0053] In the description of the present invention, it should be understood that the terms "up", "down", "front", "back", "left", "right", etc., indicating directions or positional relationships, are based on the directions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and therefore cannot be understood as a limitation on the present invention.

[0054] In the description of the present invention, it should be noted that, unless otherwise expressly specified or limited, the terms "mounted," "connected," and "connected" should be understood in a broad sense. For example, they may refer to fixed, detachable, or integral connections; mechanical or electrical connections; direct or indirect connections through an intermediate medium; and may encompass internal communication between two components or interaction between two components. Those skilled in the art will understand the specific meanings of the above terms in the present invention based on specific circumstances.

[0055] Solar cells are increasingly being used as a new energy alternative. They convert sunlight into electricity. They utilize the photovoltaic principle to generate charge carriers, which are then extracted using electrodes, facilitating efficient use of the electrical energy.

[0056] Interdigitated back contact cells, also known as IBC cells. IBC stands for Interdigitated back contact (Chinese name: Interdigitated back contact). The biggest feature of IBC cells is that the emitter and metal contact are both on the back of the cell. There is no metal electrode blocking the front, so it has a higher short-circuit current Isc. At the same time, the back can allow for wider metal grid lines to reduce the series resistance Rs and thus increase the fill factor FF. Moreover, this type of cell with no obstruction on the front not only has high conversion efficiency, but also looks more beautiful. At the same time, the full back electrode component is easier to assemble. IBC cells are one of the current technical directions for achieving high-efficiency crystalline silicon cells.

[0057] However, the preparation method of IBC cells is relatively complicated and involves many steps. Therefore, a simple method for preparing solar cells that can ensure high efficiency is needed.

[0058] To solve the above technical problems, referring to FIG. 1 to FIG. 12 , a method for manufacturing a back-contact cell is provided in an embodiment of the present invention to simplify the manufacturing process of the back-contact cell while ensuring high photoelectric conversion efficiency, including the following steps:

[0059] Step S100 , providing a substrate 10 , wherein the substrate 10 has a first surface and a second surface opposite to each other, wherein the first surface has first doped regions 101 and second doped regions 102 arranged alternately, and a third region 103 for separating the first doped regions 101 and the second doped regions 102 ;

[0060] Step S200, as shown in FIG2, sequentially forming a first interface passivation layer 14 and a first doping layer 11 on the first surface of the substrate 10;

[0061] Step S300 , as shown in FIG3 , forms a first mask layer 16 only on the surface of the first doping layer 11 located in the first doping region 101 ;

[0062] Step S400, as shown in FIG4 , removes the first doping layer 11 and the first interface passivation layer 14 located in the second doping region 102 and the third region 103; specifically, the first doping layer 11 can be removed by a dry etching method or a wet etching method, and the wet etching method includes: an alkaline solution or an acidic solution etching method. The dry etching method includes: a plasma etching method. Among them, the speed of removing the first doping layer 11 and the first interface passivation layer 14 in the second doping region 102 and the third region 103 is greater than the speed of removing the first mask layer 16. Generally speaking, etching using a method with a difference in etching speed can well realize the masking effect of the first mask layer 16.

[0063] Step S500, as shown in FIG5, a second interface passivation layer 15 and a second doping layer 12 are sequentially formed on the first mask layer 16, the second doping region 102 and the third region 103 simultaneously. The conductivity type of the second doping layer 12 is opposite to that of the first doping layer 11;

[0064] Step S600 , as shown in FIG6 , forms a second mask layer 17 only on the surface of the second doping layer 12 located in the second doping region 102 ;

[0065] Step S700, as shown in FIG7, removes the second doping layer 12 and the second interface passivation layer 15 located on the first mask layer 16 and the third region 103, and only retains the second interface passivation layer 15 and the second doping layer 12 located in the second doping region 102;

[0066] In step S800 , as shown in FIG. 10 , a first electrode 20 is formed on the first doping layer 11 , and a second electrode 21 is formed on the second doping layer 12 .

[0067] When the above technical solution is adopted, compared with the prior art, during the patterning process of the first doping layer 11 and the second doping layer 12, a mask layer is formed only in the area where the first doping layer 11 or the second doping layer 12 is required, thereby avoiding the formation of unnecessary mask layers in other areas and reducing the step of removing the mask layers in unnecessary areas. In addition, the patterning of the second doping layer 12 (i.e., the process of removing the second doping layer 12 in the area outside the second mask layer 12) and the formation of the third area 103 are completed in the same step, which simplifies the steps. In addition, when the second doping layer 12 is made and the second doping layer 12 is patterned, the first mask layer 16 is always retained on the first doping layer 11. Therefore, during the patterning process of the second doping layer 12, the alkaline solution is blocked by the first mask layer 16, so the alkaline solution cannot damage the first doping layer 11 of the first doping region 101. Due to the protective effect of the first mask layer 16 on the first doping layer 11, the patterning preparation of the first doping region 101 and the second doping region 102 is completed, reducing damage to the first doping layer 11 and ensuring the conductive performance of the first doping layer 11.

[0068] Among them, in actual applications, the substrate 10 is a semiconductor substrate 10. The material of the substrate 10 can be selected from materials such as silicon (Si) or germanium (Ge) or materials such as gallium arsenide (GaAs). Obviously, in terms of conductivity type, the substrate 10 can be an intrinsic conductive substrate, an n-type conductive substrate or a p-type conductive substrate. Preferably, the substrate 10 is a p-type conductive substrate or an n-type conductive substrate. Compared with the intrinsic conductive substrate, the p-type conductive substrate or the n-type conductive substrate has better conductivity, so that the final back-contact battery has a lower body resistivity, thereby improving the efficiency of the back-contact battery.

[0069] The first doping layer 11 and the second doping layer 12 are also semiconductor doping layers. In terms of the internal arrangement of the material, the first doping layer 11 and the second doping layer 12 can be amorphous, microcrystalline, single crystal, nanocrystalline or polycrystalline. In terms of specific materials, the materials of the first doping layer 11 and the second doping layer 12 can be silicon (Si), germanium (Ge), silicon carbide (SiC x ) or gallium arsenide (GaAs), etc. In terms of conductivity type, the first doping layer 11 and the second doping layer 12 can be n-type doping layers or p-type doping layers.

[0070] In some examples, when the substrate 10 is an n-type substrate, the first doping layer 11 can be a p-type doping layer, and the second doping layer 12 can be an n-type doping layer; or, when the substrate 10 is a p-type substrate, the first doping layer 11 can be an n-type doping layer, and the second doping layer 12 can be a p-type doping layer.

[0071] The first interface passivation layer 14 and the second interface passivation layer 15 are tunneling oxide layers. The tunneling oxide layer allows majority carriers to tunnel into the semiconductor doping layer while blocking minority carriers from passing through. Then, majority carriers are transported laterally in the semiconductor doping layer and collected by the electrode, which reduces the recombination of carriers and improves the open circuit voltage and short circuit current of the back contact battery. At this time, the tunneling oxide layer and the semiconductor doping layer constitute a tunneling oxide layer passivation contact structure, which can achieve excellent interface passivation and selective collection of carriers, thereby improving the photoelectric conversion efficiency of the back contact battery. Obviously, the tunneling oxide layer can also be replaced by other interface passivation layers. Among them, the first interface passivation layer 14 and the second interface passivation layer 15 can be one or more of oxides, nitrides, carbides, and hydrogenated amorphous silicon; among them, the oxide can be a mixture of one or more of silicon oxide, silicon oxynitride, aluminum oxide, titanium oxide, HfO2, Ga2O3, Ta2O5, and Nb2O5; among them, the nitride can be one or more of silicon nitride, aluminum nitride, TiN, and TiCN; among them, the carbide can be SiC, SiCN, etc.

[0072] The thickness of the first doping layer 11 and the second doping layer 12 are both in the range of 50 nm to 500 nm. The process of forming the first interface passivation layer 14 and the first doping layer 11 on the substrate 10 and the process of forming the second doping layer 12 on the first mask layer 16, the second doping region 102 and the third region 103 can be a plasma chemical vapor deposition (PECVD) process, a hot wire chemical vapor deposition process, a physical vapor deposition (PVD) process, a low pressure chemical vapor deposition (LPCVD) process or a catalytic chemical vapor deposition process. The process of removing the first interface passivation layer 14 and the first doping layer 11 located in the second doping region 102 and the third region 103 and removing the second doping layer 12 located in the third region 103 and the first mask layer 16 can be a laser etching process, an ion milling etching process, a plasma etching process, a reactive ion etching process, an alkali etching process or an acid etching process.

[0073] In practice, there are various methods for forming electrodes. A burn-through slurry can be directly applied to the passivation film, followed by a heat treatment to allow the electrode slurry to penetrate the passivation film and establish contact. Alternatively, a passivation film opening can be formed in a small area where contact is to be made, followed by electrode slurry application, laser transfer, electroplating, chemical plating, light-induced plating, or physical vapor deposition (PVD) methods such as evaporation and sputtering.

[0074] Obviously, electrodes can also be formed using a combination of one or more of the above methods, such as using a PVD seed layer combined with printed electrodes, or screen printing of electrode slurry combined with electroplating, or a combination of laser transfer and screen printing sintering.

[0075] For example, in the method of forming electrodes by opening a film, a contact region is formed by opening a passivation film, a P-type contact region is formed on the patterned first doping layer 11 , and an N-type contact region is formed on the patterned second doping layer 12 .

[0076] Conductive paste is printed on the contact area or backside passivation film and sintered to form metallized contacts. A P-type metal region is formed on the P-type contact area, and an N-type metal region is formed on the N-type contact area. Alternatively, a burn-through paste is printed directly on the passivation film over the patterned first and second doped regions to form the corresponding P-type and N-type metal regions.

[0077] Furthermore, after forming the electrodes, there may be other steps, such as light injection or electrical injection of carriers or other heat treatment processes, as well as efficiency grading or slicing steps.

[0078] The IBC cell with a passivated contact structure fabricated by this method has excellent passivation, minimal metal area recombination, and a simple process flow. It does not require a mask layer formed by external heating oxidation or PECVD methods, and combines the mask layer formation process with the patterning process. A two-step laser oxidation process is used to form a back-side PN passivated contact cross structure with isolated areas, significantly reducing recombination in the direct PN interface area, thereby improving cell efficiency.

[0079] Furthermore, in this embodiment, first mask layer 16 is a first oxide mask layer; and / or second mask layer 17 is a second oxide mask layer. Because both first mask layer 16 and second mask layer 17 are oxide mask layers, the oxide mask layers can be formed directly on first doped layer 11 and second doped layer 12 through oxidation. Furthermore, compared to other separately prepared mask layers, such as printed masks, oxide mask layers have a high degree of cleanliness and do not introduce other elements, thereby preventing contamination or other impacts on the first and second doped layers. Oxide masks are also easy to clean.

[0080] The oxide mask is specifically: when the first doping layer 11 and the second doping layer 12 are SiC and Si, the oxide mask formed is SiO x In the case where the first doping layer 11 and the second doping layer 12 are germanium, the oxide mask layer formed is GeO x .

[0081] As shown in Figure 11, in this embodiment, the method for forming the first oxide mask layer is: in an oxygen-containing atmosphere, laser irradiation oxidation is performed only on the surface of the first doping layer 11 located in the first doping region 101; and / or, the method for forming the second oxide mask layer is: in an oxygen-containing atmosphere, laser irradiation oxidation is performed only on the surface of the second doping layer 12 located in the second doping region 102.

[0082] In a specific implementation, the apparatus shown in FIG11 is used. Within a sealed chamber 30, an oxygen-containing atmosphere is continuously introduced through an air inlet 301 and exhausted through an exhaust port 302. A laser is irradiated in chamber 30 at a specific area of ​​a silicon-containing semiconductor substrate placed therein, thereby forming an oxide mask layer in the area scanned by the laser.

[0083] Since the oxide mask layer is formed directly on the first doping layer 11 and the second doping layer 12 by laser irradiation, the oxide mask layer is formed with high precision. Compared with the mask layer formed by external thermal oxidation or PECVD method, the heat generated during the laser irradiation process is small, thereby reducing damage to the first doping layer 11 and the second doping layer 12.

[0084] In this embodiment, the oxygen-containing atmosphere gas is one or more of oxygen, ozone, air, CO2, and N2O. Other atmosphere gases or carrier gases, such as nitrogen, may also be included. In this oxygen-containing atmosphere, laser irradiation allows the first doped layer 11 and the second doped layer 12 to undergo an oxidation reaction with the gas, forming an oxide mask layer on their surfaces.

[0085] Furthermore, the wavelength range of the laser is 190nm-545nm.

[0086] As shown in Figure 7, further, in this embodiment, in step S700, an alkaline solution is specifically used to remove the second doping layer 12 and the second interface passivation layer 5 located on the first mask layer 16 and the third region 103, and in this step, the same alkaline solution is used to continue to form a velvet structure on the third region 103 of the first surface and the second surface of the substrate 10 at the same time.

[0087] Because the patterning of the second doped layer 12, the patterning of the third region 103, and the texturing of the second surface of the substrate 10 can be completed simultaneously in the same step using the same alkaline solution, the number of process steps is greatly reduced. The textured structure of the third region 103 increases the light trapping level on the back side of the back-contact cell, thereby improving power generation when the back-contact cell is used in a bifacial module. Compared to conventional techniques, in which the second surface texturing is usually performed before the formation of the doped semiconductor layer, it is easy for the second surface texture to be damaged during the patterning or cleaning process of the doped semiconductor layer. In the present invention, the second surface texturing process is placed after the formation of the first doped layer 11 and the second doped layer 12, ensuring the integrity of the textured structure of the second surface and its light trapping performance. In particular, when the textured structure of the second surface is a nano-textured structure, various cleaning and patterning processes will almost certainly damage the nano-textured texture. In recent years, the use of nano-microstructures for texturing the light-receiving surface has become increasingly widespread, making the advantages of the post-texturing method increasingly prominent. The nanotextured texture structure has a better light-trapping effect. And because the light-receiving surface of the back-contact cell has no electrode, the color of the second surface will be more beautiful after applying the nanotextured texture structure to the back-contact cell. Therefore, the nanotextured texture structure is more suitable for back-contact cells.

[0088] Specifically, in this embodiment, at 70° C. to 90° C., an alkaline solution containing 1 wt% to 5 wt% KOH, NaOH, or tetramethylammonium hydroxide is used to remove the second doping layer 12 and the second interface passivation layer 15 located on the first mask layer 16 and the third region 103. The same alkaline solution is then used to simultaneously form a textured structure on the third region 103 and the second surface of the first surface. Under these conditions, a better etching effect can be achieved, and a uniform nano-micro textured structure can be formed.

[0089] As shown in FIG8-FIG10 , in this embodiment, forming the first electrode 20 on the first doping layer 11 and forming the second electrode 21 on the second doping layer 12 in step S800 specifically includes the following steps:

[0090] Step S801: Remove the first mask layer 16 on the first doped layer 11 and the second mask layer 17 on the second doped layer 12. After completing step S700, since the first mask layer 16 still remains on the first doped layer 11 and the second mask layer 17 still remains on the second doped layer 12, after the first mask layer 16 and the second mask layer 17 have completed their protective functions for the first doped layer 11 and the second doped layer 12, the first mask layer 16 and the second mask layer 17 can be removed before proceeding with subsequent electrode fabrication.

[0091] In step S802 , a first surface passivation layer 13 is formed simultaneously on the first doping layer 11 , the second doping layer 12 and the third region 103 .

[0092] In step S803 , a first electrode 20 is formed on the first surface passivation layer 13 of the first doping layer 11 , and a second electrode 21 is formed on the first surface passivation layer 13 of the second doping layer 12 . The first electrode 20 is in electrical contact with the first doping layer 11 , and the second electrode 21 is in electrical contact with the second doping layer 12 .

[0093] After the patterning of the first doping layer 11 and the second doping layer 12 and the formation of the third region 103 are completed, the first mask layer 16 and the second mask layer 17 can be removed to improve the conductive contact performance between the first doping layer 11 and the first electrode 20, and between the second doping layer 12 and the second electrode 21. The first surface passivation layer 13 can passivate the surface of the back contact battery, passivate the dangling bonds in the first doping layer 11, the second doping layer 12 and the third region 103, reduce the carrier recombination velocity on the first surface, and improve the photoelectric conversion efficiency. The first electrode 20 and the second electrode 21 are electrically contacted with the first doping layer 11 and the second doping layer 12 through the first opening 130 and the second opening 131 respectively, forming a local ohmic contact between the metal and the semiconductor, reducing the contact area between the metal electrode and the first doping layer 11 and the second doping layer 12, reducing the contact resistance, further reducing the carrier recombination velocity at the electrode surface, and improving the open circuit voltage.

[0094] Specifically, in practical applications, the process for forming the first surface passivation layer 13 can be a plasma chemical vapor deposition (PECVD) process, a hot wire chemical vapor deposition process, a physical vapor deposition (PVD) process, a low pressure chemical vapor deposition (LPCVD) process, or a catalytic chemical vapor deposition process. When the back-contact cell has the first surface passivation layer 13, and the first electrode 20 and the second electrode 21 are continuous contact electrodes, the method for forming the first electrode 20 and the second electrode 21 can also be to coat the electrode slurry on the first surface passivation layer 13, and then sinter it so that the electrode slurry passes through the first surface passivation layer 13 and forms electrical contact with the second doping layer 12 respectively. When a back-contact cell has a first surface passivation layer 13 and the first and second electrodes 20 and 21 are local contact electrodes, the method for forming the first and second electrodes 20 and 21 can also be to first open the first and second openings 130 and 131 in the first surface passivation layer 13, and then form the local contact first and second electrodes 20 and 21 using methods such as printing slurry, laser transfer, electroplating, chemical plating, photoinduced plating, or physical vapor deposition such as vacuum evaporation and magnetron sputtering. The opening method can include laser film opening or film opening using an etching slurry that reacts with the first surface passivation layer 13. The method of establishing electrical contact through the opening can achieve low metal area recombination in the back-contact cell, ensuring high conversion efficiency of the back-contact cell. Obviously, the first and second electrodes 20 and 21 can also be formed using a combination of one or more of the above methods. For example, a method using a physical vapor deposition (PVD) seed layer in combination with printed electrodes, screen printing of electrode slurry in combination with electroplating, or a combination of laser transfer and screen printing sintering methods can be used.

[0095] Exemplarily, as shown in Figures 8 to 10, a first electrode 20 is formed on the first doping layer 11, and a second electrode 21 is formed on the second doping layer 12, specifically: a layer of silicon nitride is deposited on the first doping layer 11, the second doping layer 12 and the third region 103 using a PECVD process as a first surface passivation layer 13; a first opening 130 is opened on the first surface passivation layer 13 located in the first doping layer 11 by laser opening, and then the first electrode 20 is formed by printing a conductive paste. A second opening 131 is opened on the first surface passivation layer 13 of the second doping layer 12 by laser opening, and then the second electrode 21 is formed by printing a conductive paste. The first electrode 20 is electrically contacted with the second doping layer 121 through the first opening 130, and the second electrode 21 is electrically contacted with the third doping layer 122 through the second opening 131.

[0096] For example, after forming the first electrode 20 and the second electrode 21 , other steps may be performed, such as optical or electrical carrier injection or other heat treatment processes, as well as efficiency binning or slicing steps.

[0097] In some examples, the step of forming the third region 103 can be set before forming the first surface passivation layer 13. The step of forming the third region 103 can also be set after the preparation of the outer city back contact cell, but this will sacrifice part of the passivation of the third region 103.

[0098] Furthermore, in this embodiment, in step S801, an etching solution containing fluorine can be used to remove the first mask layer 16 and the second mask layer 17. When the first mask layer 16 and the second mask layer 17 are silicon oxide layers, a solution containing HF or NH4F can be used to remove the silicon oxide layers. An etching solution containing fluorine can relatively easily remove mask layers, especially oxide mask layers.

[0099] In this embodiment, in step S802, the step of simultaneously forming the first surface passivation layer 13 on the first doped layer 11, the second doped layer 12, and the third region 103 further includes forming a second surface passivation layer 18 on the second surface. In this manner, the second surface passivation layer 18 is formed in the same step as the first surface passivation layer 13, simplifying the steps, and the second surface passivation layer 18 has the effects of reducing incident light reflection and passivation.

[0100] Specifically, the process for forming the second surface passivation layer 18 can be a plasma chemical vapor deposition (PECVD) process, a hot wire chemical vapor deposition process, a physical vapor deposition (PVD) process, a low pressure chemical vapor deposition (LPCVD) process or a catalytic chemical vapor deposition process.

[0101] In some examples, after forming the second surface passivation layer 18, an anti-reflection layer may be formed on the second surface passivation layer 18. The anti-reflection layer can reduce reflection of light incident on the second surface, improve light refraction, and increase the utilization rate of light incident on the second surface, thereby improving the photoelectric conversion efficiency of the back-contact cell. The surface passivation layer and the anti-reflection layer can be composed of one or more of silicon nitride, silicon oxide, silicon oxynitride, aluminum oxide, silicon carbide, and amorphous silicon.

[0102] In this embodiment, the first doped layer 11 and the second doped layer 12 are formed by an in-situ doping method or an ex-situ doping method. That is, the first doped layer 11 and the doped film layer 12 can be formed directly, or an intrinsic semiconductor layer and an intrinsic semiconductor film layer can be formed first, and then doped to form the first doped layer 11 and the doped film layer 12.

[0103] Furthermore, in this embodiment, before forming the first electrode 20 on the first doping layer 11 and forming the second electrode 21 on the second doping layer 12, the step of: performing a heat treatment process to crystallize at least a portion of the first doping layer 11 and / or the second doping layer 12. Specifically, the p-type or n-type semiconductor layer can be heat-treated to further distribute the dopant or change the structure of the semiconductor layer, which is more conducive to improving the performance of the battery. For example, when the first doping layer 11 and the second doping layer 12 are amorphous semiconductors or microcrystalline semiconductors, heating annealing can crystallize at least a portion of the first doping layer 11 and / or the second doping layer 12, thereby improving the conductivity of the first doping layer 11 and the second doping layer 12. In addition, heating annealing can also make the first interface passivation layer 14 and the second interface passivation layer 15 (such as a tunneling oxide layer) more conducive to the selective transmission of carriers; heating can also allow the doping elements to enter the tunneling oxide layer and the substrate 10, thereby reducing the transmission resistance.

[0104] Taking the manufacture of the n-type back contact cell shown in FIG1 as an example, this embodiment provides a specific manufacturing process of the n-type back contact cell:

[0105] The first step is to provide an n-type silicon substrate 10 , and then perform polishing, cleaning and other damage removal processes on the n-type silicon substrate 10 in sequence.

[0106] In the second step, as shown in FIG2 , a silicon oxide tunneling oxide layer and a boron-doped p-type polysilicon layer are deposited on the first surface of the n-type silicon substrate 10 using a PECVD device. The silicon oxide tunneling oxide layer serves as the first interface passivation layer 14 , and the boron-doped p-type polysilicon layer serves as the first doping layer 11 .

[0107] In the third step, as shown in 3 , in an oxygen-containing atmosphere, only the surface of the p-type polysilicon layer located in the first doping region 101 is irradiated with laser light to form a first oxide mask layer.

[0108] In the fourth step, as shown in FIG4 , an alkaline etching process is used to remove the p-type polysilicon layer and the silicon oxide tunneling oxide layer located in the second doping region 102 and the third region 103 , and a first doping layer 11 and a first interface passivation layer 14 are formed only on the first doping region 101 . The thickness of the first doping layer 11 is 200 nm.

[0109] In the fifth step, as shown in FIG5 , a silicon oxide tunneling oxide layer and a phosphorus-doped n-type polysilicon layer are deposited on the first oxide mask layer and the exposed second doped region 102 and the third region 103 using a PECVD device. The silicon oxide tunneling oxide layer serves as the second interface passivation layer 15, and the phosphorus-doped n-type polysilicon layer serves as the second doped layer 12.

[0110] In the sixth step, as shown in FIG6 , in an oxygen-containing atmosphere, only the surface of the n-type polysilicon layer located in the second doping region 102 is irradiated with laser light to form a second oxide mask layer.

[0111] In the seventh step, as shown in Figure 7, an alkaline etching process is used to remove the second doping layer 12 located on the third region 103 and the first oxide mask layer, leaving only the second interface passivation layer 15 and the second doping layer 12 located on the second doping region 102. The thickness of the second doping layer 12 is 200 nm. At the same time, the third region 103 and the second surface are textured using the same alkaline solution to form a suede structure.

[0112] In the eighth step, as shown in FIG8 , a fluorine-containing solution is used to remove the first oxide mask layer and the second oxide mask layer.

[0113] In the ninth step, as shown in FIG9 , a layer of silicon nitride is deposited on the first doped layer 11 , the third region 103 and the second doped layer 12 using PECVD equipment as a first surface passivation layer 13 , and a layer of silicon nitride is deposited on the velvet structure of the second surface as a second surface passivation layer 18 .

[0114] In the tenth step, as shown in FIG10 , a first opening 130 is formed in the first surface passivation layer 13 at the first doped region 101 using a laser, and then a first electrode 20 is formed by printing a conductive paste. The first electrode 20 is electrically contacted with the first doped layer 11 through the first opening 130. A second opening 131 is formed in the first surface passivation layer 13 at the second doped region 102 using a laser, and then a conductive paste is printed to form a second electrode 21. The second electrode 21 is electrically contacted with the second doped layer 12 through the second opening 131, forming the back-contact cell shown in FIG1 . Both the first electrode 20 and the second electrode 21 are local contact electrodes, each with a width of 50 μm.

[0115] In this embodiment, along the direction in which the first doping region 101 and the second doping region 102 are staggered, the width of the first doping region 101 is greater than the width of the second doping region 102. The width of the first doping region 101 is 600 μm to 2000 μm. The width of the second doping region 102 is 200 μm to 1000 μm. Based on this, the width of the first doping layer 11 on the first doping region 101 is greater than the width of the second doping layer 12 on the second doping region 102, and the width range of the formed pn junction is also larger, that is, the area for carrier separation is relatively large, which is conducive to carrier separation and thus improves the photoelectric conversion efficiency of the battery. Preferably, the width range of the first doping region 101 is between 600 μm and 1500 μm, and the width range of the second doping region 102 is between 200 μm and 800 μm.

[0116] For example, the width of the first doping region 101 may be 600 μm, and the width of the second doping region may be 500 μm; or, the width of the first doping region 101 may be 2000 μm, and the width of the second doping region may be 200 μm; or, the width of the first doping region 101 may be 1400 μm, and the width of the second doping region may be 1000 μm.

[0117] In some examples, the width of the third region 103 ranges from 10 μm to 100 μm along the direction in which the first doping region and the second doping region are staggered. If the third region 103 is too wide, the effective area of ​​the back contact battery may be wasted, and effective carriers may be difficult to collect, thereby reducing battery performance. The third region 103 is arranged between the first doping region 101 and the second doping region 102, so that the first doping region 101 and the second doping region 102 are separated from each other at the boundary, eliminating the insulator design between the positive electrode and the negative electrode in the prior art, which can reduce the production process flow and the spatial complexity. Such a structure will not have the coexistence of positive and negative electrodes in the vertical direction, thus avoiding the occurrence of leakage in the back contact battery; it can also improve the reliability performance of the battery in later products and reduce the difficulty of the production process of the back contact battery.

[0118] Illustratively, the width of the third region may be 10 μm, 100 μm, or 60 μm.

[0119] As some possible implementations, as shown in FIG1 , the surface of the first doping region 101 and / or the surface of the second doping region 102 is a polished surface.

[0120] Based on this, the surfaces of the first doped region 101 and the second doped region 102 can both be polished surfaces, so that light incident from the second surface and passing through the back contact cell is re-reflected, so that the light has the opportunity to be reused by the back contact cell, thereby improving the photoelectric conversion efficiency of the back contact cell. In addition, the polished surface has better flatness, and the subsequent formation of other layers on the polished surface will have a better effect, which is conducive to reducing the generation of interface defects, thereby reducing the recombination of carriers caused by defects, and is conducive to improving the passivation performance of the back contact cell, thereby improving the photoelectric conversion efficiency of the back contact cell.

[0121] The IBC battery with a passivated contact structure fabricated by this method boasts excellent passivation, minimizes metal area recombination, and simplifies the process flow. It eliminates the need for a mask layer formed by external heated oxidation or PECVD, combining the mask layer formation process with a patterning process. A laser oxidation process is employed to form a back-side PN passivated contact cross structure with a third region, significantly reducing recombination in the direct PN interface region, thereby improving battery efficiency. In the description of the aforementioned embodiments, specific features, structures, materials, or characteristics may be combined in any suitable manner in any one or more embodiments or examples.

[0122] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any modifications or substitutions that can be easily conceived by a person skilled in the art within the technical scope disclosed in the present invention should be included in the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be based on the scope of protection of the claims.

Claims

1. A method for manufacturing a back contact battery, characterized in that: include: Providing a substrate, the substrate having a first surface and a second surface opposite to each other, the first surface having first doped regions and second doped regions arranged alternately, and a third region for spacing the first doped regions and the second doped regions; forming a first interface passivation layer and a first doping layer in sequence on the first surface of the substrate; forming a first mask layer only on the surface of the first doping layer located in the first doping region; removing the first doping layer and the first interface passivation layer located on the second doping region and the third region; forming a second interface passivation layer and a second doping layer simultaneously and sequentially on the first mask layer, the second doping region and the third region, wherein the second doping layer has a conductivity type opposite to that of the first doping layer; forming a second mask layer only on the surface of the second doping layer located in the second doping region; removing the second doping layer and the second interface passivation layer located on the first mask layer and the third region, and retaining only the second interface passivation layer and the second doping layer located in the second doping region; A first electrode is formed on the first doping layer, and a second electrode is formed on the second doping layer.

2. The method for manufacturing a back contact battery according to claim 1, wherein: The first mask layer is a first oxide mask layer; and / or the second mask layer is a second oxide mask layer.

3. The method for manufacturing a back contact battery according to claim 2, wherein: The first oxide mask layer is formed by: performing laser irradiation oxidation only on the surface of the first doping layer located in the first doping region in an oxygen-containing atmosphere; and / or The second oxide mask layer is formed by performing laser irradiation oxidation only on the surface of the second doping layer located in the second doping region in an oxygen-containing atmosphere.

4. The method for manufacturing a back contact battery according to claim 3, wherein: The gas in the oxygen-containing atmosphere is one or more of oxygen, ozone, air, CO2, and N2O.

5. The method for manufacturing a back contact battery according to claim 1, wherein: The second doping layer and the second interface passivation layer on the first mask layer and the third region are removed using an alkaline solution, and a textured structure is continuously formed on the third region of the first surface and the second surface simultaneously using the same alkaline solution.

6. The method for manufacturing a back contact battery according to claim 5, characterized in that: At 70°C to 90°C, an alkaline solution of KOH, NaOH or tetramethylammonium hydroxide with a mass percentage of 1% to 5wt% is used to remove the second doping layer and the second interface passivation layer located on the first mask layer and the third region, and the same alkaline solution is used to continue to form a velvet structure on the third region of the first surface and the second surface at the same time.

7. The method for manufacturing a back contact battery according to claim 1, wherein: The step of forming the first electrode on the first doping layer and forming the second electrode on the second doping layer specifically includes the steps of: removing the first mask layer located on the first doping layer and the second mask layer located on the second doping layer; forming a first surface passivation layer on the first doped layer, the second doped layer and the third region simultaneously; A first electrode is formed on the first surface passivation layer located on the first doping layer, and a second electrode is formed on the first surface passivation layer located on the second doping layer, wherein the first electrode is in electrical contact with the first doping layer, and the second electrode is in electrical contact with the second doping layer.

8. The method for manufacturing a back contact battery according to claim 6, wherein: removing the first mask layer and the second mask layer using an etching solution containing fluorine; and / or, The step of simultaneously forming the first surface passivation layer on the first doping layer, the second doping layer and the third region further includes forming a second surface passivation layer on the second surface.

9. The method for manufacturing a back contact battery according to claim 1, wherein: The first doping layer and the second doping layer are formed by an in-situ doping method or an ex-situ doping method.

10. The method for manufacturing a back contact battery according to claim 1, wherein: Before the steps of forming the first electrode on the first doping layer and forming the second electrode on the second doping layer, the method further includes performing a heat treatment process to crystallize at least a portion of the first doping layer and / or the second doping layer.