CORRUGATED CARDBOARD MATERIAL

VN10062379BActive Publication Date: 2026-10-19OJI HLDG CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
VN1202401087
Authority / Receiving Office
VN · VN
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-04-21
Filing Date
2021-03-30
Publication Date
2026-10-19
Estimated Expiration
2041-03-30

AI Technical Summary

Technical Problem

Corrugated cardboard materials often experience issues with folding retention and line cracking, leading to instability and damage in packaged boxes, particularly due to gaps between sheets and weak creases, which can result in tears and poor packaging quality.

Method used

A corrugated cardboard material with a liner bonded to a core, featuring specific dynamic viscoelastic properties, sizing agents, paper strength enhancers, and fiber length optimization to ensure folding retention, prevent line cracking, and enhance the strength of the liner, thereby improving packaging stability and resistance to tears.

Benefits of technology

The solution effectively maintains folded states, suppresses line cracking, and prevents tears in boxes, ensuring regularity and stability of packaging, even under humid conditions, by optimizing the dynamic viscoelasticity and composition of the cardboard material.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a corrugated cardboard material (1) which is a corrugated cardboard material consisting of a liner attached to an intermediate layer, in which the dynamic elastic viscosity measured on a measuring piece cut from the liner by a tensile sliding method at a frequency of 100Hz under a temperature of 25°C is within a predetermined range. The dynamic elastic viscosity is determined by the elastic modulus E' and the tanδ value which is the ratio of the loss modulus E to the elastic modulus E''. The predetermined range includes: elastic modulus E' greater than or equal to 1.00 × 109Mpa and less than or equal to 8.00 × 109Mpa, and tanδ greater than or equal to 2.50 × 10-2 and less than or equal to 1.50 × 10-1.
Need to check novelty before this filing date? Find Prior Art

Description

Cardboard material

[0001] The present invention relates to corrugated board materials.

[0002] Concertina-folded (also known as "fanfold") corrugated cardboard is a well-known box-making material. The corrugated cardboard has folds between successive rectangular sheets, and the sheets are folded back alternately along these folds. In this type of corrugated cardboard, successive sheets are stacked one on top of the other and folded into a rectangular package shape.

[0003] The folding device for manufacturing the above-mentioned accordion-folded cardboard material includes a folding part that alternately folds successive sheets along fold lines, and a stacking part that stacks the folded sheets (see, for example, Patent Document 1 listed below). In order to ensure the stability and regularity of the package shape of the manufactured cardboard material, it is desirable that the successive sheets are folded together in the stacking part so that they are in contact with each other across the fold lines without any gaps.

[0004] The above-mentioned cardboard material is used as packaging material in a box-making system (also called an "automatic packaging system," "variable three-side system," "automatic three-side packaging," or "on-demand packaging") that produces boxes of the optimum size depending on the size of the packaged item. This box-making system performs the following various processes (see Patent Document 2 below): Feeding process: a process of feeding out accordion-folded cardboard material; Cutting process: a process of cutting out flat cardboard material fed out in the feeding process; Folding process: a process of assembling a box from the cardboard material cut out in the cutting process; Printing process: a process of printing on flat or assembled cardboard material; and Packing process: a process of placing contents into the assembled box.

[0005] Special Publication No. 2015-509473 Publication Special Publication No. 2013-513869

[0006] However, depending on the properties of the cardboard material, gaps may occur between consecutive sheets at the folds ("fold opening"), resulting in insufficient ability to maintain the folded state of the sheets (fold retention). This, in turn, may result in insufficient stability and shapeability of the package. Furthermore, depending on the properties of the cardboard material, breakage (crease cracks) may occur at the folds when the sheets are folded. Furthermore, when cardboard material with folds, such as accordion-folded cardboard, is used as a material for a box-making system, depending on the properties of the sheets used for the cardboard material, the manufactured box may be prone to tearing (breakage). Furthermore, with cardboard material with folds, such as accordion-folded cardboard, depending on the properties of the sheets used for the cardboard material, tearing (crease cracks) may occur at the folds. This invention was invented in consideration of the above-mentioned problems, and one of its objectives is to achieve both sufficient fold retention and the prevention of crease cracks. Another object of the present invention is to prevent boxes made from cardboard from breaking (damage). Another object of the present invention is to prevent creases at folds. However, other objects of the present invention are not limited to these objects. The functions and effects derived from the various configurations shown in the "Mode for Carrying Out the Invention" below, which cannot be obtained with conventional technology, can also be considered as other objects of the present invention.

[0007] (1) The cardboard material disclosed herein is a cardboard material using a cardboard with a liner laminated to a core. The dynamic viscoelasticity of this cardboard material, measured on a test piece cut out from the liner in a tensile shear mode under vibration conditions of a temperature of 25°C and a frequency of 100 Hz, falls within a predetermined range, and the dynamic viscoelasticity is defined by the values ​​of elastic modulus E' and tan δ, which is the ratio of loss modulus E" to elastic modulus E'. The predetermined range is when the elastic modulus E' is 1.00 x 10 9 [MPa] or more and 8.00 × 10 9 [MPa] or less, and the tan δ is 2.50 × 10 -2 or more and 1.50 × 10 -1 The following is the result.

[0008] (2) The cardboard material disclosed herein is a cardboard material using a cardboard having a liner laminated to a core, wherein the amount of sizing agent added to the liner is 0.2 parts by mass or more and 4.0 parts by mass or less, the amount of paper strength agent added to the liner is 0.1 parts by mass or more and 4.0 parts by mass or less, the average fiber length of the pulp fibers constituting the liner is 0.90 mm or more and 1.55 mm or less, and the content of fine fibers having a fiber length of 0.0 mm or more and 0.2 mm or less among the pulp fibers constituting the liner is 23% or more and 48% or less.

[0009] (3) The cardboard material disclosed herein is a cardboard material using a cardboard in which a liner is bonded to a core. The cardboard material has a liner density of 0.60 [g / cm 3 ] or more and 0.85 [g / cm 3 ] or less, the average fiber length of the pulp fibers constituting the liner is 0.98 [mm] or more and 1.55 [mm] or less, and the amount of fine fibers having a fiber length of 0.0 [mm] or more and 0.2 [mm] or less among the pulp fibers constituting the liner is 15 [%] or more and 38 [%] or less.

[0010] (1) This invention can ensure both the ability to keep the fold and the prevention of crease cracking. (2) This invention can prevent damage to boxes made from cardboard. (3) This invention can prevent crease cracking at the fold.

[0011] Fig. 1 is a perspective view showing a bellows-folded cardboard material; Fig. 2 is an explanatory diagram explaining a folding mechanism; Fig. 3 is an explanatory diagram showing a packaging style of a bellows-folded cardboard material, showing a good packaging style; Fig. 4 is an explanatory diagram showing a packaging style of a bellows-folded cardboard material, showing an improper packaging style.

[0012] The following describes a cardboard material as an embodiment. The cardboard material mainly exemplified in this embodiment is a box-making material in which a rectangular sheet is folded into a continuous corrugated cardboard. For this cardboard material, a double-sided cardboard with liners on both sides of the core is used.

[0013] The above-mentioned double-sided corrugated board includes not only single-flute corrugated board made of three base papers (materials) corresponding to one corrugating medium and two liners, but also multi-flute corrugated board made of five or more base papers corresponding to three or more corrugating mediums and two liners, such as so-called "double-sided corrugated board" or "triple-sided corrugated board." In this embodiment, a corrugated board material made of single-flute double-sided corrugated board is mainly exemplified.

[0014] When cardboard material is made into a box, it becomes a cardboard box. More specifically, the cardboard material used as the box-making material in the box-making system is made into a cardboard box through various processes, such as a feeding process in which sheets are fed out in sequence, a cutting process in which the fed sheets are cut out into the unfolded pattern of the box, and a folding process in which the sheets are folded into the shape of the box. The box-making system that assembles the cardboard box is not particularly limited, and examples of fully automatic packaging systems that can be used include the "Cartonwrap 1000 manufactured by CMC Corporation," the "CVP-500 manufactured by Neopost Corporation," and the "TXP-600 manufactured by OS Machinery Co., Ltd.", as well as semi-automatic systems such as the "EM7 manufactured by Pack Size Corporation" and the "Compack manufactured by Panotec Corporation."

[0015] In this embodiment, an example is given in which the following directions I and II correspond as shown in Table 1 below, and the cardboard material is placed on a horizontal surface. Direction I: Direction in the cardboard material placed on a horizontal surface Direction II: Direction in the semi-finished product in the middle of manufacturing the cardboard material

[0016]

[0017] The machine direction (first direction, denoted as "CD" in the drawings) and the cross direction (second direction, denoted as "MD" in the drawings) are horizontal directions along which the plane of the sheet (fold) extends. These machine direction and cross direction are perpendicular to each other. The height direction (third direction, denoted as "TD" in the drawings) is a vertical direction and is perpendicular to both the machine direction and the cross direction. This height direction corresponds to the direction in which the sheets are stacked.

[0018] The MD (Machine Direction) direction is also called the "flow direction" and is the direction in which the manufacturing process of cardboard material progresses from upstream to downstream. The CD (Cross Direction) direction is the direction perpendicular to the MD direction in a plane along the MD direction. The TD (Transverse Direction) direction is the direction perpendicular to both the MD direction and the CD direction. In addition, unless otherwise specified, the expression "numerical value X to numerical value Y" in this embodiment means a range equal to or greater than numerical value X and equal to or less than numerical value Y.

[0019] [I. One Embodiment] In the following one embodiment, the configuration of the cardboard material is described in items [1] and [2]. Item [1] describes the structure of the cardboard material folded (hereinafter referred to as the "folded structure"). Item [2] describes parameters related to the properties of the sheet (corrugated cardboard sheet) used for the cardboard material. Then, item [3] describes the actions and effects of the configurations of items [1] and [2].

[0020] [1. Folding Structure] As shown in Fig. 1, the cardboard material 1 is a rectangular parallelepiped box-making material. In the cardboard material 1, continuous rectangular sheets 2 (only some of which are marked with reference numerals in Fig. 1) are folded back at folds F (only some of which are marked with reference numerals in Fig. 1), and the folded sheets 2 are stacked in the height direction. In the cardboard material 1 folded in this manner, a plurality of folds F extend linearly in the length direction on a pair of side surfaces along both the length direction and the height direction.

[0021] Here, the folding structure of the cardboard material 1 will be explained, focusing on three continuous sheets 2 (shown by two-dot chain lines in FIG. 1). First sheet 21: Sheet 2 continuous with one side of the second sheet 22 Second sheet 22: Sheet 2 continuous with both the first sheet 21 and the third sheet 23 Third sheet 23: Sheet 2 continuous with the other side of the second sheet 22

[0022] A first fold F1 is provided between the first sheet 21 and the second sheet 22, and the sheets 21 and 22 are continuous with each other via the first fold F1. A second fold F2 is provided between the second sheet 22 and the third sheet 23, and the sheets 22 and 23 are continuous with each other via the second fold F2. The first fold F1 is a fold F at which the second sheet 22 is folded back toward one side of the lateral direction (to the right in FIG. 1 ) relative to the first sheet 21, and is located on the other side of the lateral direction (to the left in FIG. 1 ) of the cardboard material 1. The second fold F2 is a fold F at which the third sheet 23 is folded back toward the other side of the lateral direction (to the left in FIG. 1 ) relative to the second sheet 22, and is located on the other side of the lateral direction (to the right in FIG. 1 ) of the cardboard material 1.

[0023] In the first sheet 21, the corrugations 10 (waves) of the cardboard are exposed at a first edge E1 (only the front edge is marked with a reference symbol in FIG. 1 ) extending in the horizontal direction (direction intersecting with the fold F). Similarly, in the second sheet 22, the corrugations 10 of the cardboard are exposed at a second edge E2 (only the front edge is marked with a reference symbol in FIG. 1 ) extending in the horizontal direction (direction intersecting with the fold F). In the sheet pair 20 consisting of the first sheet 21 and the second sheet 22, the first edge E1 and the second edge E2 are arranged adjacent to each other in the height direction.

[0024] With the cardboard material 1 having the above-described folding structure, even materials that are difficult to roll up can be folded into a rectangular parallelepiped shape. In other words, cardboard sheets 2 that are stronger than materials that can be rolled up can be packed in a compact form. The cardboard material 1, in which the sheet 2 is folded to ensure strength in this way, is suitable for use as packaging material in a box-making system that produces boxes that require strength.

[0025] In addition, the folds F are provided along the corrugations 10 of the cardboard. In other words, the cardboard material 1 is produced with corrugations 10 perpendicular to the MD direction. The cardboard material 1 is preferably wrapped (wrapped) in a wrapping film to prevent it from being soiled or collapsed.

[0026] [2. Parameters] The following describes the parameters of the cardboard material 1. First, basic parameters such as the size and number of layers of the cardboard material 1 will be described. After that, parameters related to the sheet 2 of the cardboard material 1 will be described in detail.

[0027] [2-1. Basic Parameters] The size of the cardboard material 1 is determined by the following dimensions L1 to L3. - Vertical dimension L1: Vertical dimension (first dimension) - Horizontal dimension L2: Horizontal dimension (second dimension) - Height dimension L3: Height dimension (third dimension) The smaller the dimensions L1 to L3, the greater the restrictions on the size and shape of the boxes to be manufactured, and the larger they are, the greater the risk of reduced workability in transportation and delivery. From these perspectives, it is preferable that dimensions L1 to L3 be within the ranges shown in Table 2 below.

[0028]

[0029] Furthermore, if the number of folds F in the cardboard material 1 is N, then the number of sheets 2 is N+1. In this case, N+1 layers of sheets 2 are stacked in the cardboard material 1. For example, the number of layers of the cardboard material 1 can be various, ranging from 10 to 1,000 layers. For cardboard materials for which folding-related parameters are measured, as will be described in detail later, it is preferable to measure the parameters for each layer for measurement targets with less than a predetermined number of layers (e.g., 100 layers). On the other hand, for measurement targets with a predetermined number of layers (e.g., 100 layers) or more, the parameters may be measured partially (e.g., in sections divided into parts or in a set area).

[0030] The sheet 2 used for the cardboard material 1 can be set to any basis weight. The basis weight range adopted for the sheet 2 is 50 to 1500 [g / m2 ], and preferably 100 to 1000 [g / m 2 ], and more preferably 200 to 800 [g / m 2 ], and more preferably 200 to 600 [g / m 2 The weight of the cardboard material 1 is calculated by taking into account the run rate of the core and multiplying the length L1, width L2, and the number of rows N+1 of the sheet 2 into the basis weight.

[0031] [2-2. Parameters Related to Properties] <Configuration A> The cardboard material 1 of this embodiment has configuration A related to properties, based on the viewpoint of improving the packaging appearance of the cardboard material 1. Specifically, it has a predetermined configuration A related to properties, based on the following viewpoints I and II. "Packaging appearance of the cardboard material 1" refers to the appearance of the cardboard material 1 in an accordion-like fold folded into a rectangular parallelepiped. Viewpoint I: Ensuring the ability to retain the fold at the fold F Viewpoint II: Suppressing crease cracks at the fold F The above viewpoints I and II are viewpoints for solving the following problems I and II. Problem I: The fold opens at the fold F. Problem II: Crease cracks occur at the fold F

[0032] The "fold retention" referred to in the above viewpoint I refers to the ability to maintain the state in which the sheet 2 is folded at the fold F. The "unfolding at the fold F" referred to in problem I refers to the fact that when the sheet 2 is folded at the fold F, the folded state is not maintained and a gap is created between consecutive sheets 2 through the fold F. Problem I occurs when the fold retention is insufficient. Problem I can also be said to be the problem in which the packaging shape of the cardboard material 1 becomes distorted when the sheet 2 is folded at the fold F. The "crease crack" referred to in the above viewpoint II and problem II refers to a crack (break, tear) that occurs in the liner located outside the fold F when the sheet 2 is folded at the fold F.

[0033] Attempting to ensure fold retention based on viewpoint I tends to make problem II more likely to occur, while attempting to suppress crease cracking at fold F based on viewpoint II tends to make problem I more likely to occur. Therefore, it is difficult to achieve both viewpoint I and viewpoint II. Below, as prerequisites for viewpoints I and II, the configuration of the folding device that produces accordion-folded cardboard material 1 and the quality of the packaging of the produced cardboard material 1 will be explained in subsections [i] and [ii]. Then, in subsection [iii], a specific configuration based on viewpoints I and II will be explained.

[0034] [i. Folding device] The folding device 50 shown in Fig. 2 is a device that folds a continuous strip of cardboard into an accordion-like shape. The folding device 50 is not particularly limited, but for example, the following folding device can be used. Folding device: Model number "AS-F" manufactured by BHS Corrugated Machinery Co., Ltd.

[0035] The folding device 50 includes a conveying part 50A, a folding part 50B, and a stacking part 50C. The conveying part 50A forms a conveying path for conveying a strip-shaped cardboard web 1W produced by an upstream cardboard production device (corrugator) (not shown) to the folding part 50B (see the two-dot chain line in FIG. 2).

[0036] A corrugated cardboard web 1W produced by a corrugator (not shown) has multiple folds F spaced at regular intervals in the horizontal direction. Sheets 2 (see FIG. 1) are continuous with each other on the upstream and downstream sides of each fold F. The multiple folds F include folds in which the upstream sheet is folded back in one horizontal direction (to the right in FIG. 2) relative to the downstream sheet (folds corresponding to the "first fold F1" in FIG. 1), and folds in which the upstream sheet is folded back in the other horizontal direction (to the left in FIG. 2) relative to the downstream sheet (folds corresponding to the "second fold F2" in FIG. 1). These first folds F1 and second folds F2 are alternately arranged in the conveyance direction.

[0037] The surface facing upward in the conveying part 50A is referred to as the front surface of the cardboard web 1W, and the surface facing downward is referred to as the back surface of the cardboard web 1W. The first fold F1 is formed by a groove recessed in the front surface of the cardboard web 1W, and the second fold F2 is formed by a groove recessed in the back surface of the cardboard web 1W, thereby ensuring folding in each of the above directions.

[0038] The folding part 50B is provided between the conveying part 50A and the stacking part 50C, and alternately folds the cardboard web 1W conveyed by the conveying part 50A at folds F and feeds it to the stacking part 50C. In the folding part 50B, the cardboard web 1W conveyed from the conveying part 50A falls downward while being pushed out in the conveying direction. At this time, at the first fold F1, the upstream sheet is folded back in one lateral direction (to the right in FIG. 2 ) relative to the downstream sheet, and at the second fold F2, the upstream sheet is folded back in the other lateral direction (to the left in FIG. 2 ) relative to the downstream sheet.

[0039] The folding part 50B may be provided with an assisting mechanism (not shown) that assists in folding back the cardboard web 1W. The assisting mechanism is a mechanism that assists in ensuring that the sheets that make up the cardboard web 1W are alternately folded back at the first fold F1 and the second fold F2. The specific structure of the assisting mechanism is not particularly limited, but for example, a rotating mechanism (see Patent Document 1 above) equipped with a rod that supports the second fold F2 can be used.

[0040] The stacking part 50C is a part that stacks the sheets that have been alternately folded in the folding part 50B. The stacking part 50C is located below the folding part 50B. Therefore, in the stacking part 50C, the sheets 2 (see FIG. 1) that have been alternately folded at folds F1 and F2 are stacked sequentially from bottom to top. In this way, the accordion-folded cardboard material 1 that has a rectangular parallelepiped package shape is manufactured.

[0041] 3A, in a cardboard material 1 with a good packaging condition, successive sheets are folded back 180° at fold F, and then the successive sheets are folded together with no gaps between them at fold F. If fold F is kept closed in this manner, the cardboard material 1 has a good packaging condition, but there is a risk of problem II occurring, in which the fold F may break.

[0042] In a poorly packaged cardboard material 1, as shown in FIG. 3B , consecutive sheets are folded 180° at fold F, and then a gap S is created between the consecutive sheets at fold F, and the subsequent sheets are stacked. If fold F is not maintained closed in this manner, cracks at fold F are unlikely to occur, but there is a risk of problem I occurring, in which the fold at fold F opens. This can cause the sheets to fold at the gap S or the cardboard material 1 to tilt above the gap S, potentially impairing the shape and stability of the cardboard material 1. Ultimately, the stacked sheets may collapse during the accordion-folding process, potentially preventing the creation of an accordion-folded cardboard material 1.

[0043] [iii. Structure] The cardboard material 1 has the following structure 1A as structure A corresponding to the above-mentioned viewpoints I and II and problems I and II. Structure 1A: The dynamic viscoelasticity of the liner constituting the cardboard material 1 is within a predetermined range. "Dynamic viscoelasticity" is a parameter defined by three values: elastic modulus E', loss modulus E'', and tan δ. This parameter corresponds to the ability of the cardboard material 1 to maintain its folded state when folded (how difficult it is to open the fold F) and the resistance to cracking at the fold F. When the cardboard material 1 is folded at the fold F, the pulp fibers constituting the liner base paper of the cardboard material 1 are stretched, and "dynamic viscoelasticity" can also be said to be a parameter corresponding to the ability of the pulp fibers to maintain their stretched state when the cardboard material 1 is folded at the fold F.

[0044] The elastic modulus E' represents the strength of elasticity and corresponds to the repulsive force that tries to return to its original shape when the cardboard material 1 is folded (i.e., tries to open the fold F). The loss modulus E'' represents the strength of viscosity. Tan δ is the ratio of the loss modulus E'' to the elastic modulus E', as calculated in the following formula 1. If tan δ is a value of 1 or less, it means that the material has physical properties in the elastic region (a region that tries to return to its original shape), and if it is not, it means that the material has physical properties in the viscous region (a region that has difficulty returning to its original shape). tan δ = E'' / E' Formula 1 The larger the value of tan δ, the smaller the repulsive force, and the smaller the value of tan δ, the greater the repulsive force.

[0045] The inventors of the present application have found that the above-mentioned problems I and II tend to be suppressed if the elastic modulus E' and tan δ of the dynamic viscoelasticity of the liner constituting the cardboard material 1 are within a predetermined range. Conversely, they have found that cardboard material using a liner with dynamic viscoelasticity outside the predetermined range tends to be prone to problems I and II. In other words, the cardboard material 1 is provided with the above-mentioned configuration 1A based on the above-mentioned viewpoints I and II.

[0046] If the modulus of elasticity E' of the dynamic viscoelasticity exceeds a specified range and tan δ is below a specified range, when the cardboard material 1 is folded at the crease F, the pulp fibers that make up the liner base paper do not remain stretched, and the repulsive force that tries to open the crease F increases, presumably leading to Problem I. If the modulus of elasticity E' of the dynamic viscoelasticity is below a specified range and tan δ is above a specified range, when the cardboard material 1 is folded at the crease F, the pulp fibers that make up the liner base paper are stretched, and an external force due to bending is applied to the crease F, presumably making it more likely to lead to Problem II.

[0047] The elastic modulus E' is 1.00 x 10 9 [MPa] or more and 8.00 × 10 9 [MPa] or less, and tan δ is 2.50 × 10 -2 or more and 1.50 × 10 -1If the values ​​of the elastic modulus E' and tan δ are within these ranges, a corrugated cardboard material suitable for box making can be obtained. In terms of suitability for manufacturing accordion-folded corrugated cardboard, a modulus of elasticity E' of 1.50 × 10 9 [MPa] or more and 7.00 × 10 9 [MPa] or less, and tan δ is preferably 3.00 × 10 -2 or more than 1.00 × 10 -1 In terms of suitability as a material for use in an automatic packaging system, it is preferable that the elastic modulus E′ is 2.00×10 or less. 9 [MPa] or more and 6.00 × 10 9 [MPa] or less, and tan δ is preferably 3.50 × 10 -2 or more, 9.70 × 10 -2 More preferably, it is:

[0048] Furthermore, based on viewpoint I, the elastic modulus E' is 3.00 × 10 9 [MPa] or less and tan δ is 7.00 × 10 -2 It is preferable that the elastic modulus E' is 2.50 × 10 or more. 9 [MPa] or less and tan δ is 8.00 × 10 -2 Based on viewpoint II, it is more preferable that the elastic modulus E′ is 4.00×10 or more. 9 [MPa] or more and tan δ is 4.00 × 10 -2 It is preferable that the elastic modulus E' is 4.50 × 10 or less. 9 [MPa] or more and tan δ is 3.80 × 10 -2 More preferably, it is:

[0049] <Configuration B> Furthermore, the cardboard material 1 of this embodiment has a property-related configuration B based on the viewpoint of being able to manufacture boxes that are less likely to break when used as a box-making material. Specifically, it has a predetermined property-related configuration B based on the following viewpoint III. - Viewpoint III: Suppressing breakage (damage) of assembled boxes The above viewpoint III is a viewpoint for solving the following problem III. - Problem III: Assembled boxes are likely to break

[0050] When accordion-folded cardboard material 1 is used as a box-making material in a box-making system (automated packaging system), folds F may be included on the bottom or sides of the assembled box. In boxes assembled using accordion-folded cardboard material 1, tears tend to occur easily starting from the folds F. Therefore, the above-mentioned problem I can be said to be a problem that easily leads to tears in boxes assembled using accordion-folded cardboard material 1. Tears starting from the folds F tend to occur more easily under humid conditions. Therefore, the above-mentioned problem I can be said to be a problem that easily leads to tears in boxes assembled using accordion-folded cardboard material 1 under humid conditions.

[0051] The cardboard material 1 has the following configurations B1 to B4 as configuration B corresponding to the above-mentioned viewpoint III and problem III. Configuration B1: The amount of sizing agent added is within a predetermined range. Configuration B2: The amount of paper strength agent added is within a predetermined range. Configuration B3: The average fiber length of the fiber length is within a predetermined length range. Configuration B4: The amount of fine fibers is within a predetermined range.

[0052] The "sizing agent" is a chemical that is added to the liner that constitutes the cardboard material 1 to impart surface properties such as sizing ability (the ability to prevent water penetration and ink bleeding) and printability to the liner. The amount of sizing agent added [parts by mass] is the ratio of the amount of sizing agent added [parts by mass] to the total of 100 [parts by mass] of all pulp that constitutes the liner. The "paper strength agent" is a chemical that is added to the liner that constitutes the cardboard material 1 to improve the surface strength of the liner and prevent the generation of paper dust during printing. The amount of paper strength agent added [parts by mass] is the ratio of the amount of paper strength agent added [parts by mass] to the total of 100 [parts by mass] of all pulp that constitutes the liner.

[0053] The "length average fiber length" is the average length (fiber length) of the pulp fibers that make up the liner. This length average fiber length is the average length of pulp fibers, including the fine fibers described below. The "fine fiber content" is the percentage (%) of the amount of fine fibers contained in the liner relative to the total (100%) of the pulp fibers that make up the liner. Here, fine fibers are fine fibers with a fiber length of 0.0 mm or more and 0.2 mm or less.

[0054] The inventors of the present application have found that the above-mentioned Problem III tends to be suppressed if the liner constituting the cardboard material 1 has the above-mentioned features B1 to B4. Conversely, they have found that cardboard material using a liner that does not have at least one of the above-mentioned features B1 to B4 tends to cause Problem III. In other words, the cardboard material 1 has the above-mentioned features B1 to B4 based on the above-mentioned Viewpoint III.

[0055] If the amount of sizing agent added is below the specified range, if the amount of strength agent added is below the specified range, or if the average fiber length is below the specified length range, the strength of the liner is insufficient, and it is presumed that this will lead to Problem III. If the amount of sizing agent added exceeds the specified range, the sizing agent inhibits hydrogen bonding between the pulp fibers that make up the liner, which is presumed to lead to Problem III. The strength of the liner tends to increase as the amount of strength agent added increases, but if the amount of strength agent added exceeds the specified range, the strength agent aggregates and the strength decreases, which is presumed to lead to Problem III.

[0056] The longer the average fiber length, the stronger the liner tends to be, but if the average fiber length exceeds a certain length range, the gaps between the pulp fibers increase, which is thought to lead to Problem III. In particular, under humid conditions, the gaps between the pulp fibers are more likely to absorb water, which is thought to make Problem III more likely to occur.

[0057] It is presumed that if the amount of fine fibers is below the predetermined range, the proportion of pulp fibers with long fiber length (long fibers) increases, increasing the gaps between the long fibers, resulting in Problem III. It is presumed that, particularly under humid conditions, water is more likely to be absorbed in the gaps between the long fibers, making Problem III more likely to occur. It is presumed that if the amount of fine fibers is above the predetermined range, the proportion of long fibers decreases, reducing the entanglement of the pulp fibers, resulting in Problem III.

[0058] The amount of sizing agent added is 0.2 parts by mass to 4.0 parts by mass, preferably 0.5 parts by mass to 3.0 parts by mass, and more preferably 0.8 parts by mass to 2.0 parts by mass. The amount of paper strength amplifier added is 0.1 parts by mass to 4.0 parts by mass, preferably 0.5 parts by mass to 3.5 parts by mass, and more preferably 1.0 parts by mass to 3.0 parts by mass.

[0059] The length-average fiber length is 0.90 mm or more and 1.55 mm or less, preferably 1.00 mm or more and 1.53 mm or less, and more preferably 1.30 mm or more and 1.52 mm or less. The fine fiber content is 23% or more and 48% or less, preferably 30% or more and 47% or less, and more preferably 40% or more and 46% or less.

[0060] <Configuration C> The cardboard material 1 of this embodiment has a property-related configuration C based on the viewpoint of preventing tears (creases) from occurring at the fold F. Specifically, it has a predetermined property-related configuration C based on the following viewpoint IV. - Viewpoint IV: Suppressing creases at the fold F The above viewpoint IV is a viewpoint for solving the following problem IV. - Problem IV: Creases are likely to occur at the fold F In accordion-folded cardboard material 1, fold F is the point where the continuous sheet is folded back 180°. In accordion-folded cardboard material 1, creases tend to occur at this fold F. Therefore, the above problem IV can be said to be a problem that makes creases likely to occur at the fold F in accordion-folded cardboard material 1. The cardboard material 1 has the following configurations C1 to C3 as configuration C corresponding to the above viewpoint IV and problem IV. Configuration C1: The liner density is within a predetermined range. Configuration C2: The average fiber length of the fiber is within a predetermined length range. Configuration C3: The amount of fine fibers is within a predetermined range.

[0061] "Density" refers to the volume of the liner that forms the cardboard material 1 [cm 3 ] is a parameter that represents the weight [g] per [unit]. The "length average fiber length" is the average length (fiber length) of the pulp fibers that make up the liner. This length average fiber length is the average length of pulp fibers including the fine fibers described below. The "fine fiber content" is the percentage [%] of the amount of fine fibers contained in the total pulp fibers that make up the liner (100 [%]). Here, fine fibers are fine fibers with a fiber length of 0.0 [mm] or more and 0.2 [mm] or less.

[0062] The inventors of the present application have found that if the liner of the cardboard material 1 has the above-mentioned features C1 to C3, the above-mentioned problem IV tends to be suppressed. Conversely, they have found that cardboard material using a liner that does not have at least one of the above-mentioned features C1 to C3 tends to be more susceptible to problem IV. In other words, the cardboard material 1 has the above-mentioned features C1 to C3 based on the above-mentioned aspect IV.

[0063] It is presumed that if the density is below the specified range, many gaps will occur between the pulp fibers, making the liner insufficient in strength, resulting in Problem IV. If the density is above the specified range, the gaps between the pulp fibers will disappear, making it difficult for stress to escape when the liner is bent, resulting in Problem IV. The shorter the average fiber length, the more the strength of the liner tends to decrease, and if the average fiber length is below the specified length range, the strength of the liner will be insufficient, resulting in Problem IV.

[0064] The longer the average fiber length, the greater the strength of the liner tends to be, but if the average fiber length exceeds a specified length range, unevenness in the distribution of pulp fibers is likely to occur, resulting in areas of locally low strength, which is presumably causing Problem IV. If the amount of fine fibers is below the specified range, the proportion of pulp fibers with long fiber lengths (long fibers) increases, increasing the gaps between the long fibers, which is presumably causing Problem IV. If the amount of fine fibers exceeds the specified range, the proportion of long fibers decreases, reducing the entanglement of pulp fibers, resulting in insufficient liner strength, which is presumably causing Problem IV.

[0065] The density of the liner is 0.60 [g / cm 3 ] or more and 0.85 [g / cm 3 ] or less, and preferably 0.65 [g / cm 3 ] or more and 0.84 [g / cm 3 ] or less, and more preferably 0.80 [g / cm 3 ] or more and 0.83 [g / cm 3 The length-average fiber length is 0.98 mm or more and 1.55 mm or less, preferably 1.00 mm or more and 1.53 mm or less, and more preferably 1.10 mm or more and 1.52 mm or less. The fine fiber content is 15% or more and 38% or less, preferably 17% or more and 37% or less, and more preferably 18% or more and 36% or less.

[0066] [3. Actions and Effects] (1) By including the above-described configuration A, the cardboard material 1 of this embodiment does not unfold at the fold F when folded back at the fold F, and crease cracks are unlikely to occur at the fold F. This makes it possible to ensure both the ability to maintain the fold and the prevention of crease cracks. Therefore, for example, the regularity and stability of the package shape can be ensured with the accordion-folded cardboard material 1.

[0067] (2) Furthermore, by providing the above-described configuration B, the cardboard material 1 of this embodiment ensures the strength of the liner that constitutes the cardboard material 1, thereby preventing the box manufactured using the cardboard material 1 from breaking. In particular, tearing originating from the fold F under humid conditions can be prevented.

[0068] (3) Furthermore, since the cardboard material 1 of this embodiment has the above-mentioned configuration C, the strength of the liner that constitutes the cardboard material 1 is ensured, and tearing (creasing) of the cardboard material 1 at the fold F can be suppressed.

[0069] [II. Examples] Hereinafter, the structures A, B, and C of the present invention will be specifically explained using examples and comparative examples. However, the present invention is not limited to the following examples. In the examples and comparative examples, the cardboard material whose parameters are measured (hereinafter referred to as the "measured cardboard material") is a double-sided cardboard sheet. This measured cardboard material has the following dimensions: Size: length 1300 [mm], width 1150 [mm], height 1800 [mm]

[0070] <Configuration A> First, we will describe examples related to Configuration A. In Examples A1 to A6 and Comparative Examples A7 and A8, one of the following three types of flutes was used: A flute B flute E flute

[0071] In each of Examples A1 to A6 and Comparative Examples A7 and A8, one of the following liner base papers "No. 1" to "No. 6" was used for the front liner and the back liner. No. 1: Basis weight 120 [g / m 2], freeness 400 [ml] No. 2: basis weight 160 [g / m 2 ], freeness 400 [ml] No. 3: basis weight 170 [g / m 2 ], freeness 400 [ml] No. 4: basis weight 210 [g / m 2 ], freeness 400 [ml] No. 5: basis weight 120 [g / m 2 ], freeness 300 [ml] No. 6: basis weight 120 [g / m 2 ], freeness 600 [ml]

[0072] The liner base paper of product number "No. 1" was made from softwood kraft pulp with a freeness of 400 ml and recycled cardboard pulp, and was produced as a three-layer cardboard liner base paper by papermaking using a multi-layer papermaking machine. The papermaking conditions were as follows: a cationic paper strength agent was contained in an amount of 0.5 parts by mass relative to 100 parts by mass of the total pulp in the paper layers, and softwood kraft pulp was contained in a proportion of 10% by mass of the pulp in the surface layer. All of the cationic paper strength agent was contained in the surface layer. The softwood kraft pulp accounted for 6% by mass of the total pulp in the paper layers.

[0073] The liner base paper of product number "No. 2" has a basis weight of 160 [g / m 2 The liner paper of product number "No. 3" was produced in the same manner as the liner paper of "No. 1", except that the content of softwood kraft pulp in the surface layer pulp was changed to 50 [mass %] and the basis weight was changed to 170 [g / m 2 The liner paper of product number "No. 4" was produced in the same manner as the liner paper of "No. 1", except that the basis weight was changed to 210 [g / m 2 ] was changed to "No. 1" and the same method was used to prepare the liner base paper.

[0074] The liner paper of product number "No. 5" was produced in the same manner as the liner paper of "No. 1", except that the freeness of the softwood kraft pulp and the recycled cardboard pulp was changed to 300 ml. The liner paper of product number "No. 6" was produced in the same manner as the liner paper of "No. 1", except that the freeness of the softwood kraft pulp and the recycled cardboard pulp was changed to 600 ml.

[0075] "Freeness" is a parameter that indicates the degree to which the pulp, which is the raw material for base paper, has been beaten. Beating pulp is a mechanical process in which pulp fibers are beaten and ground (grinded), and is carried out using a well-known refiner (mechanical processing equipment). The freeness value can be adjusted by changing the refiner's settings. The process of beating pulp (beating process) is carried out immediately before the papermaking process in the base paper manufacturing process. In this beating process, in addition to beating the pulp used in papermaking, treatments such as compounding chemicals with the pulp are also carried out.

[0076] In each of Examples A1 to A6 and Comparative Examples A7 and A8, one of the following core raw papers, "No. 7" and "No. 8", was used for the core. No. 7: Basis weight 120 [g / m 2 ] [OND-EM120: manufactured by Oji Materia Co., Ltd.] No. 8: Basis weight 160 [g / m 2 ] [OND-EM160: manufactured by Oji Materia Co., Ltd.] The measurement cardboard materials of Examples A1 to A6 and Comparative Examples A7 and A8 were double-sided cardboard having the total thickness [mm] shown in Table 3.

[0077]

[0078] For each of the above Examples A1 to A6 and Comparative Examples A7 and A8, the dynamic viscoelasticity (three values ​​of elastic modulus E', loss modulus E'' and tanδ) shown in Table 3 was measured. In each of Examples A1 to A6 and Comparative Examples A7 and A8, the value of elastic modulus E' was changed by adjusting the freeness of the liner base paper, and as a result, the value of tanδ was adjusted.

[0079] The dynamic viscoelasticity was measured using measurement sample pieces (measurement pieces) taken out from the measurement cardboard materials of Examples A1 to A6 and Comparative Examples A7 and A8 according to the following procedures A1 to A5.

[0080] Step A1: Cut out a measurement sheet from any row above the middle row, based on half the total number of rows (i.e., the middle row) of the cardboard material to be measured. Specifically, if the total number of rows M of the cardboard material to be measured is odd, cut out a sheet based on the row obtained by rounding up or down half the total number of rows (i.e., the middle row). If the total number of rows M of the cardboard material to be measured is even, cut out a sheet based on half the total number of rows [(M / 2) + 1] of the total number of rows of the cardboard material to be measured. Note that when cutting out the sheet, care was taken to select rows that had no (or few) scratches or dents. Step A2: Immerse the measurement sheet cut out in Step A1 in tap water for 15 minutes. Step A3: The measurement sheet immersed in step A2 is removed from the tap water, and each of the liner base papers (front liner and back liner) of the removed measurement sheet is peeled off by hand, being careful not to tear the liner base papers, to separate them from the core base paper. Step A4: The liner base paper separated in step A3 is dried in a dryer at 105° for 20 minutes. Step A5: A measurement sample piece having the following dimensions is cut out from the liner base paper dried in step A4. >Dimensions - Vertical direction: 5 [mm] - Horizontal direction: 30 [mm]

[0081] The dynamic viscoelasticity (elastic modulus E', loss modulus E'', tan δ) of the measurement sample pieces cut out in step A5 above was measured using the following equipment under the following conditions. Measurements were performed using measurement sample pieces cut out from the liner base paper of the front liner. Even when measurement sample pieces cut out from the liner base paper of the back liner were used, there was no or almost no difference in the measurement results compared to when measurement sample pieces of the front liner were used. > Equipment Dynamic viscoelasticity measuring device Manufactured by UBM Co., Ltd., Model Rheogel-E4000 > Conditions Measurement method: Tensile shear mode Frequency: 100 [Hz] (oscillation condition) Strain: 0.10 [%] Temperature: 25 [°C] (temperature condition)

[0082] Evaluation: For Examples A1 to A6 and Comparative Examples A7 and A8 whose dynamic viscoelasticity was measured as described above, stackability and creaseability were evaluated as described below. "Stackability" is an evaluation criterion corresponding to the quality of the packaging when the measured cardboard material is folded accordion-like (stacked), and can also be considered the ability to maintain the sheet folded back at the crease (fold retention). "Creaseability" is an evaluation criterion corresponding to the resistance to breakage (crease cracking) at the crease when the measured cardboard material is folded back at the crease. Breakage includes cracks, tears, and tears in the liner base paper at the crease. The crease refers to the area including the periphery of the crease.

[0083] The test cardboard material to be evaluated was produced by folding a double-sided cardboard web produced by the following manufacturing process into an accordion-like fold in the following folding process. The manufacturing process includes the following steps B1 to B4. A well-known corrugator equipped with a single facer and a double facer is used to produce the double-sided cardboard web in this manufacturing process.

[0084] Step B1: Corrugations (waves) are formed in the corrugation medium raw paper supplied from the corrugation medium raw paper roll, and adhesive is applied to the crests of the corrugations formed. Step B2: Back liner raw paper supplied from the back liner raw paper roll is laminated to the corrugation medium raw paper coated with adhesive in Step B1, and the two are bonded together by applying pressure and heat with a roll to form a single-sided corrugated cardboard web (processing with a single facer). Step B3: Front liner raw paper supplied from the front liner raw paper roll is laminated with adhesive to the corrugation medium side of the single-sided corrugated cardboard web formed in Step B2, and the two are bonded together by applying pressure and heat with a pressure and heat roll to form a double-sided corrugated cardboard web (processing with a double facer). Step B4: Folds extending in the width direction are formed in the double-sided corrugated cardboard web formed in Step B3, spaced at regular intervals in the extension direction.

[0085] In the above steps B2 and B3, the pressing and heating are carried out under the following conditions, for example: > Step B2 (single facer) - Heating temperature 120 to 200°C - Roll linear pressure 20 to 40 kN / m - Pressing time 0.01 to 0.20 seconds > Step B3 (double facer) - Heating temperature 120 to 200°C - Roll linear pressure 0.1 to 1.0 kN / m - Pressing time 2 to 7 seconds

[0086] In steps B1 and B2, a commonly used one-tank starch glue was used as the adhesive used to bond the liner paper and core paper. Note that emulsions of synthetic resins may also be used to bond the liner paper and core paper. Specific examples of synthetic resins include polyethylene, polypropylene, polyamide, polyester, ethylene-unsaturated carboxylic acid copolymers, styrene-butadiene copolymers, butadiene-acrylonitrile copolymers, styrene-butadiene-acrylonitrile copolymers, polyvinyl acetate, ethylene-vinyl acetate copolymers, polyacrylic acid ester copolymers, and styrene-acrylic acid ester copolymers.

[0087] Other methods for bonding the liner paper and core paper in steps B1 and B2 include forming an adhesive layer on the liner paper or core paper by extrusion laminating or coating with a synthetic resin emulsion, and then polymerizing the liner paper and core paper, or placing a synthetic resin film between the liner paper and core paper and applying pressure and heat to bond them together.

[0088] The double-sided cardboard web produced in the above manufacturing process is folded accordion-folded in a folding process including the following steps C1 and C2. In this folding process, the following folding device is used under the following conditions: Folding device: Model number "AS-F" manufactured by BHS Corrugated Machinery Co., Ltd. Conveying speed: 100 [m / min] Step C1: After step B4, the produced double-sided cardboard web is transported to the above folding device (see transport part 50A in Figure 2). Step C2: The double-sided cardboard web transported in step C1 is folded alternately along the fold lines to produce a cardboard material for measuring the accordion-folded packaging dimensions described above (see folding part 50B and stacking part 50C in Figure 2).

[0089] In the evaluation of stackability, the appearance of the test cardboard material produced in the above procedure C2 was visually inspected and rated according to the following criteria: ○: The test cardboard material could be produced, and no gaps (see symbol S in Figure 3B) occurred in any of the folds. △: The test cardboard material could be produced, but gaps (see symbol S in Figure 3B) occurred in one or more folds. ×: The test cardboard material could not be produced. In the evaluation of stackability, a rating of "△" or better was considered good.

[0090] In the evaluation of creaseability, the measured cardboard material prepared in step C2 above was visually inspected for cracks at the folds, and the results were evaluated according to the following criteria. As mentioned above, the "folds" refers to the area including the periphery of the folds. ○: No creases were observed at any of the folds. △: One or more crease cracks were observed in a portion of the width direction at one or more folds. ×: One or more crease cracks were observed across the entire width at one or more folds. In the evaluation of creaseability, "△" or better was considered a good rating.

[0091] In Examples A1 to A6, the elastic modulus E' was 1.00 x 10 9 [MPa] or more and 8.00 × 10 9 [MPa] or less, and tan δ is 2.50 × 10 -2 or more and 1.50 × 10 -1 The stacking property and the creasing property were evaluated as "Fair" or better. In particular, the elastic modulus E' was 3.00 x 10 9 [MPa] or less and tan δ is 7.00 × 10 -2 In the above Examples A1, A2, A5, and A6, the creasing property was evaluated as "△", but the stacking property was evaluated as "◯". 9 [MPa] or more and tan δ is 4.00 × 10 -2 In the following Examples A3 and A4, stacking ability was evaluated as "△", but creasing ability was evaluated as "◯".

[0092] On the other hand, the elastic modulus E' is 1.00 × 10 9 [MPa] or less than 8.00 x 10 9 [MPa] and tan δ is 2.50 × 10 -2 Less than or 1.50 x 10 -1 In Comparative Examples A7 and A8, where the modulus of elasticity E' was greater than 8.00 x 10, the stacking property or the creasing property was evaluated as "x". 9 [MPa] and tan δ is 2.50 × 10 -2In Comparative Example A7, where the elastic modulus E' was less than 1.00 x 10, the creasing property was evaluated as "good", but the stacking property was evaluated as "poor". 9 [MPa] or less, tan δ is 1.50 × 10 -1 In the larger comparative example A8, stackability was evaluated as "good", but creasing ability was evaluated as "poor".

[0093] In consideration of Comparative Examples A7 and A8, Examples A1 to A6 show that the elastic modulus E' is 1.00 × 10 9 [MPa] or more and 8.00 × 10 9 [MPa] or less, and tan δ is 2.50 × 10 -2 or more and 1.50 × 10 -1 If the modulus of elasticity E' is 3.00 × 10 or less, it can be said that when the cardboard material to be measured is folded back at the fold, opening at the fold is suppressed and cracking at the fold is suppressed. 9 [MPa] or less and tan δ is 7.00 × 10 -2 If the elastic modulus E' is 4.00 x 10 or more, it can be said that when the cardboard material to be measured is folded back at the fold, the folded back part at the fold can be prevented from unfolding. 9 [MPa] or more and tan δ is 4.00 × 10 -2 If the thickness is less than this, it can be said that cracks at the fold line can be prevented when the cardboard material to be measured is folded back along the fold line.

[0094] From Comparative Example A7, the elastic modulus E' was 8.00 × 10 9 [MPa] and tan δ is 2.50 × 10 -2 It is presumed that, when folded at the crease, the pulp fibers constituting the liner base paper do not remain stretched, and the repulsive force that tries to open the crease increases, resulting in poor stackability. 9 [MPa] or less, tan δ is 1.50 × 10 -1 It is presumed that because the diameter is larger, the pulp fibers that make up the liner base paper are stretched and external force is applied to the fold F due to bending, resulting in poor creasing properties.

[0095] In addition, from Comparative Example A7, which has a smaller freeness value than Examples A1 to A6, and Comparative Example A8, which has a larger freeness value than Examples A1 to A6, it can be seen that the smaller the freeness value, the larger the elastic modulus E' and the smaller the value of tan δ, and the larger the freeness value, the smaller the elastic modulus E' and the larger the value of tan δ. In view of Comparative Examples A7 and A8, from Examples A1 to A6, it can be seen that if the freeness value is 350 [ml] or more and 500 [ml] or less, the elastic modulus E' is 1.00 × 10 9 [MPa] or more and 8.00 × 10 9 [MPa] or less, and tan δ is 2.50 × 10 -2 or more and 1.50 × 10 -1 It can be said that it is adjusted within the following range.

[0096] Among Examples A1 to A6, which have the same freeness, Example A3, which has a different softwood kraft pulp content and a different liner base paper basis weight from Example A1, and Example A4, which has a different liner base paper basis weight from Example 1, suggest that the greater the softwood kraft pulp content and the greater the liner base paper basis weight, the greater the elastic modulus E' and the smaller the tan δ value. 8 [MPa] or more and 2.50 × 10 8 It is presumed that the pressure is preferably in the range of 0.1 [MPa] or less.

[0097] <Configuration B> Next, an embodiment relating to configuration B will be described.

[0098] In Examples B1 to B19 and Comparative Examples B20 to B29, one of the following three types of flutes was used: A flute (single flute), total thickness: 5.0 mm; E flute (single flute), total thickness: 1.5 mm; AB flute (double flute), total thickness: 8.5 mm.

[0099] In each of Examples B1 to B19 and Comparative Examples B20 to B29, one of the following liner base papers, "No. 1" to "No. 25", was used for the front liner and the back liner. The liner base papers, "No. 1" to "No. 25", had the following basis weights and densities. No. 1: Basis weight 120 [g / m 2 ], density 0.8 [g / cm 3 ] ・No. 2, No. 6-25: Basis weight 170 [g / m 2 ], density 0.8 [g / cm 3 ] ・No. 3: Basis weight 210 [g / m 2 ], density 0.8 [g / cm 3 ] ・No. 4: Basis weight 280 [g / m 2 ], density 0.8 [g / cm 3 ] ・No. 5: Basis weight 170 [g / m 2 ], density 0.6 [g / cm 3 ]

[0100] The liner paper with product number "No. 1" was made from softwood kraft pulp and recycled cardboard pulp with a freeness of 300 ml, and was made into a three-layer cardboard liner paper using a multi-layer papermaking machine under the following papermaking conditions. The freeness was measured in accordance with JIS P8121 2012 using the following measuring device. Measuring device: Product name "Canadian Standard Freeness", Kumagai Riki Kogyo Co., Ltd., Product number "No. 2580-A".

[0101] - Papermaking conditions for product number "No. 1" > Sizing agent: "Sizepine N-830 (manufactured by Arakawa Chemical Industries, Ltd.)" ("α" in Tables 4 to 7 below) was contained at 0.3 parts by mass per 100 parts by mass of all pulp in the paper layers. > Paper strength agent: "PT-1001 (manufactured by Arakawa Chemical Industries, Ltd.)" was contained at 0.2 parts by mass per 100 parts by mass of all pulp in the paper layers. > Aluminum sulfate: was contained at 5 parts by mass per 100 parts by mass of all pulp in the paper layers. > Softwood kraft pulp: was contained at 10% by mass of the pulp fiber in the surface layer. The softwood kraft pulp accounted for 6% by mass of the total pulp in the paper layers. > Fine fiber content: was 33% of the pulp fiber making up the liner. The surface layer of the three layers of liner base paper was produced under the above papermaking conditions. The papermaking conditions for the middle layer and the back layer of the three layers of the liner base paper are not limited to the above papermaking conditions.

[0102] The liner base paper of product number "No. 2" has a basis weight of 170 [g / m 2 The liner paper of product number "No. 3" was produced in the same manner as the liner paper of "No. 1", except that the basis weight was changed to 210 [g / m 2 The liner paper of product number "No. 4" was produced in the same manner as the liner paper of "No. 1", except that the basis weight was changed to 280 [g / m 2 ] was changed to "No. 1" and the same method was used to prepare the liner base paper.

[0103] Each of the liner base papers No. 5 to No. 25 was produced in the same manner as the liner base paper No. 2, except for the following: No. 5: Density was 0.6 [g / cm 3 ] No. 6: The amount of fine fibers was changed to 25 [%] and the length average fiber length was changed to 1.08 [mm]. No. 7: The amount of fine fibers was changed to 45 [%] and the length average fiber length was changed to 0.95 [mm]. No. 8: The content of softwood kraft pulp in the surface layer pulp was changed to 20 [mass %] and the length average fiber length was changed to 1.50 [mm].

[0104] No. 9: The amount of sizing agent added was changed to 3 parts by mass. No. 10: The amount of sizing agent added was changed to 5 parts by mass. No. 11: The name of the sizing agent was changed to "Sizepine NT-78 (manufactured by Arakawa Chemical Industries, Ltd.)" (referred to as "β" in Tables 4 to 7 below). No. 12: The name of the sizing agent was changed to "Sizepine K-287 (manufactured by Arakawa Chemical Industries, Ltd.)" (referred to as "γ" in Tables 4 to 7 below). No. 13: The amount of paper strength agent added was changed to 1.5 parts by mass.

[0105] No. 14: The amount of paper strength agent added was changed to 3.0 parts by mass. No. 15: The amount of fine fibers was changed to 38% and the average fiber length was changed to 0.98 mm. No. 16: The proportion of recycled cardboard pulp in the surface layer pulp was changed to 100% by mass. No. 17: The amount of fine fibers was changed to 45% and the average fiber length was changed to 0.95 mm, and the amount of sizing agent added was changed to 5.0 parts by mass.

[0106] No. 18: The amount of fine fibers was changed to 20% and the average fiber length was changed to 1.12 mm. No. 19: The amount of fine fibers was changed to 50% and the average fiber length was changed to 0.94 mm. No. 20: The proportion of softwood kraft pulp in the surface layer pulp was changed to 20% by mass and the average fiber length was changed to 1.60 mm. No. 21: No sizing agent was added.

[0107] No. 22: The amount of sizing agent added was changed to 8.0 parts by mass. No. 23: No paper strength agent was added. No. 24: The amount of paper strength agent added was changed to 5.0 parts by mass. No. 25: The content of softwood kraft pulp in the surface layer pulp was changed to 20% by mass, the amount of sizing agent added was changed to 8.0 parts by mass, the amount of fine fibers was changed to 50% by mass, and the average fiber length was changed to 1.60 mm.

[0108] In addition, when measuring the concentration of various chemicals contained in the liner paper, such as sizing agents and paper strength additives, the chemical concentration (relative to pulp weight ratio) was measured using a pyrolysis gas chromatograph mass spectrometer (pyrolysis device: PY-2020D manufactured by Frontier Labs, gas chromatograph mass spectrometer: 5973N manufactured by Agilent Technologies). Then, the liner paper to be analyzed was peeled from the core paper according to the following procedures D1 and D2, and after drying, the liner paper was pulverized in a pulverizer. Two samples of 200 to 300 μg of the pulverized material were measured using the pyrolysis gas chromatograph mass spectrometer.

[0109] In the pyrolysis gas chromatograph mass spectrometer, the peaks of the target drugs obtained when the calibration curve was created were used as a reference. The peak areas were extracted, and the peak areas were compared with the calibration curve to calculate the drug concentration of the target drug. This measurement was performed twice for each sample, and the average value was used as the drug concentration (weight ratio to pulp). The calibration curve samples were prepared by impregnating various drugs into filter paper (Advantec, circular qualitative filter paper, No. 2) and drying the paper so that the drug concentrations were 0.01%, 0.1%, 1%, 5%, and 10% by weight. Each calibration curve sample was pulverized, and 200-300 μg of the pulverized material was applied to the pyrolysis gas chromatograph mass spectrometer to create the calibration curve.

[0110] In the above product number "No. 5," the density was changed by adjusting the nip pressure of the multi-layer paper machine. In the above product numbers "No. 6" to "No. 8," "No. 15," "No. 17" to "No. 20," and "No. 25," the amount of fine fibers and the average fiber length were adjusted using a fiber classifier (MAX-F700, manufactured by Aikawa Iron Works Co., Ltd.). In product numbers "No. 7" and "No. 17," the fiber classifier was used to remove pulp fibers other than fine fibers.

[0111] In each of Examples B1 to B19 and Comparative Examples B20 to B29, one of the following core raw papers, "No. 26" and "No. 27", was used for the core. No. 26: Basis weight 120 [g / m 2], density 0.65 [g / cm 3 ] [OND-EM120: manufactured by Oji Materia Co., Ltd.] No. 27: Basis weight 160 [g / m 2 ], density 0.65 [g / cm 3 ] [OND-EM160: manufactured by Oji Materia Co., Ltd.] For each of the above Examples B1 to B19 and Comparative Examples B20 to B29, the liner fiber information shown in Tables 4 to 7 was measured. Note that there is a possibility of a measurement error of approximately plus or minus 10% in the measured values ​​of various parameters such as density, length-average fiber length, fine fibers, and basis weight, as well as the number of parts by mass of sizing agent and paper strength agent.

[0112]

[0113]

[0114]

[0115]

[0116] "Liner fiber information" is information measured about the pulp fibers that make up the liner base paper, and includes three types: "Runkel ratio," "average fiber length," and "fine fiber content." The Runkel ratio is a parameter that indicates the shape of the pulp fiber, and is calculated as (Runkel ratio) = (twice the fiber wall thickness) / (fiber lumen diameter). A higher Runkel ratio indicates a more rigid fiber. The average fiber length is the average length (fiber length) of the pulp fibers that make up the liner. The fine fiber content is the percentage (%) of the amount of fine fibers contained relative to the total (100%) of the pulp fibers that make up the liner. Fine fibers are fine fibers with a fiber length of 0.0 mm or more and 0.2 mm or less.

[0117] The three types of "liner fiber information," namely, "Runkel ratio," "average fiber length," and "fine fiber content," were measured using the following procedures D1 to D5. Procedure D1: The second-highest layer of cardboard material was cut into a 40-cm square, and this 40-cm square cardboard sheet was used for measurement. The cutout was located in the center of the cardboard sheet's width. The cardboard sheet was then immersed in ion-exchanged water for 15 minutes and removed from the ion-exchanged water. Procedure D2: The liner base paper (front liner and back liner) from the cardboard sheet removed in Procedure D1 was separated from the core base paper by manually peeling them off, taking care not to tear the liner base paper. Procedure D3: The liner base paper and core base paper separated in Procedure D2 were each immersed in ion-exchanged water, adjusted to a concentration of 2%, and soaked for 24 hours. Procedure D4: The liner base paper and core base paper whose concentrations have been adjusted in Procedure D3 are each soaked for 24 hours, and then disintegrated for 20 minutes using a standard disintegrator (manufactured by Kumagai Riki Kogyo Co., Ltd.) to break down the pulp into fibers. Procedure D5: The slurry (pulp fibers) disintegrated in Procedure D4 was sampled, and the "Runkel ratio," "average fiber length," and "fine fiber content" were measured using the following fiber length measuring device. Fiber length measuring device: Part number FS-5 UHD base unit, manufactured by Valmet

[0118] Evaluation The tearability of the evaluation boxes for Examples B1 to B19 and Comparative Examples B20 to B29, for which the "Runkel ratio," "average fiber length," and "fine fiber content" had been measured as described above, was evaluated. "Tearability" is an evaluation standard corresponding to the weight of the load that the box can withstand for the contents housed in it. This tearability was evaluated by a load test following the following procedures E1 to E6. Procedure E1: A developed pattern for the evaluation box was cut out from the measurement cardboard material in the following shape and size using a sample cutter (CF2-1218, manufactured by Mimaki Engineering Co., Ltd.). > Shape: Pattern of an A-type corrugated cardboard box unfolded > Size: Width of side panels of A-type corrugated cardboard box: 356 [mm], Width of end panels of A-type corrugated cardboard box: 159 [mm], Height of A-type corrugated cardboard box: 256 [mm] - Step E2: Using the unfolded pattern cut out in Step E1, manually score a crease (fold) to the following depth using the following scoring jig in the area that will form the bottom of the evaluation box, and assemble the evaluation box by hand. > Scoring jig: R crease (score width: 2 [mm], manufactured by Nippon Die Steel Co., Ltd.) > Scoring depth: Depress by 50 [%] of the total thickness of the cardboard material to be measured - Step E3: The evaluation box assembled in Step E2 is treated for 1 [hour] under the following temperature and humidity conditions A. > Temperature and humidity condition A: temperature 30°C, humidity 90% Rh. Procedure E4: After processing in procedure E3, a weight weighing 15 kg is placed in the evaluation box under the above temperature and humidity condition A. The weight is placed so that the weight is applied to the entire bottom surface of the evaluation box. Procedure E5: After procedure E4, two workers lift the evaluation box and hold it for 30 seconds. Procedure E6: Visually check whether any tears have occurred in the evaluation box in procedure E5.

[0119] The tearability was evaluated according to the following criteria: 5: The bottom of the evaluation box remains unchanged. 4: No tear occurs in the bottom of the evaluation box, but dents or folds occur on the bottom (inner liner of the evaluation box). 3: No tear occurs in the bottom of the evaluation box, but dents or folds occur on the bottom (both inner and outer liners of the evaluation box). 2: A tear occurs on the bottom of the evaluation box (inner liner of the evaluation box). 1: A large tear occurs in the evaluation box while the box is being lifted and held, causing the weight to fall off the box. According to the above criteria, a rating of "3" or higher was considered good, and a rating of "2" or lower was considered bad.

[0120] The load test under the temperature and humidity condition A described above is a wet test to evaluate the tearability of the evaluation box under humid conditions. For each of the measurement cardboard materials of Examples B1 to B19 and Comparative Examples B20 to B29, in addition to the wet test, the tearability of the evaluation box was also evaluated in a load test (dry test) under dry conditions of the temperature and humidity condition B described below. > Temperature and humidity condition B: temperature 23°C, humidity 50% Rh The dry test was the same as the above procedures E1 to E6, except that temperature and humidity condition A was changed to the above temperature and humidity condition B in procedures E3 and E4.

[0121] In Examples B1 to B19, the amount of sizing agent added was 0.2 parts by mass or more and 4.0 parts by mass or less, the amount of paper strength agent added was 0.1 parts by mass or more and 4.0 parts by mass or less, the average fiber length of the pulp fibers was 0.90 mm or more and 1.55 mm or less, the amount of fine fibers was 23% or more and 48% or less, and the tearability was rated "3" or higher under both temperature and humidity conditions A and B, and the evaluation box did not tear or the weight fell.

[0122] Examples B11, B12, and B19, in which the amount of sizing agent added was 0.8 parts by mass or more, Examples B15 and B16, in which the amount of paper strength agent added was 1.0 parts by mass or more, Example 10, in which the average fiber length was 1.50 mm or more, and Examples B9 and B19, in which the amount of fine fibers was 40% or more, were evaluated as "4" or higher under temperature and humidity condition A.

[0123] On the other hand, in comparative examples B20 to B29, in which the amount of sizing agent added was less than 0.2 parts by mass or more than 4.0 parts by mass, the amount of paper strength agent added was less than 0.1 parts by mass or more than 4.0 parts by mass, the average fiber length of the pulp fibers was less than 0.90 mm or more than 1.55 mm, or the amount of fine fibers was less than 23% or more than 48%; a rating of "2" or less was obtained at least under temperature and humidity condition A.

[0124] In light of Comparative Examples B20 to B29, Examples B1 to B19 indicate that breakage (damage) of boxes manufactured using the measured cardboard material can be suppressed if the amount of sizing agent added is 0.2 parts by mass or more and 4.0 parts by mass or less, the amount of paper strength agent added is 0.1 parts by mass or more and 4.0 parts by mass or less, the average fiber length of pulp fibers is 0.90 mm or more and 1.55 mm or less, and the fine fiber content is 23% or more and 48% or less. Furthermore, Examples B9, B10, B11, B12, B15, B16, and B19 indicate that breakage (damage) can be prevented under humid conditions if the amount of sizing agent added is 0.8 parts by mass or more, the amount of paper strength agent added is 1.0 parts by mass or more, the average fiber length is 1.50 mm or more, and the fine fiber content is 40% or more.

[0125] From Comparative Examples B26 and B29, it is presumed that the amount of sizing agent added of more than 4.0 parts by mass inhibits hydrogen bonding between fibers, reducing the strength of the liner under humid conditions and making it more susceptible to tearing. From Comparative Example B28, it is presumed that the amount of paper strength agent added of more than 4.0 parts by mass causes the paper strength agent to aggregate, reducing the strength of the liner and making it more susceptible to tearing. From Comparative Examples B24 and B29, it is presumed that the length-average fiber length is greater than 1.55 mm, creating large gaps between the long fibers that make the liner more susceptible to water absorption, reducing the strength of the liner under humid conditions and making it more susceptible to tearing. From Comparative Example B20, it is presumed that the amount of fine fibers added of less than 23% creates large gaps between the long fibers that make the liner more susceptible to water absorption, reducing the strength of the liner under humid conditions and making it more susceptible to tearing. From comparative examples B21 to B23 and B29, it is presumed that when the amount of fine fibers is greater than 48%, the amount of long fibers is reduced and the pulp fibers are less entangled, resulting in a decrease in the strength of the liner and making it more susceptible to tearing.

[0126] <Configuration C> Next, an example relating to Configuration C will be described. In the example relating to Configuration C, the cardboard material to be measured was prepared by manually folding a strip-shaped cardboard web in an accordion-like manner to the above-mentioned size by an operator.

[0127] In Examples C1 to C11 and Comparative Examples C12 to C19, one of the following three types of flutes was used: A flute (single flute), total thickness: 5.0 mm; E flute (single flute), total thickness: 1.5 mm; AB flute (double flute), total thickness: 8.2 mm.

[0128] In each of Examples C1 to C11 and Comparative Examples C12 to C19, one of the following liner base papers, "No. 1" to "No. 15", was used for the front liner and the back liner. The liner base papers, "No. 1" to "No. 15", had the following basis weights and densities. No. 1: Basis weight 120 [g / m 2 ], density 0.8 [g / cm 3] ・No. 2, No. 6 to 11: Basis weight 170 [g / m 2 ], density 0.8 [g / cm 3 ] ・No. 3: Basis weight 210 [g / m 2 ], density 0.8 [g / cm 3 ] ・No. 4: Basis weight 280 [g / m 2 ], density 0.8 [g / cm 3 ] ・No. 5: Basis weight 170 [g / m 2 ], density 0.7 [g / cm 3 ] ・No. 12, 14: Basis weight 170 [g / m 2 ], density 0.5 [g / cm 3 ] ・No. 13,15: Basis weight 170 [g / m 2 ], density 0.9 [g / cm 3 ]

[0129] The liner paper with product number "No. 1" was made from softwood kraft pulp and recycled cardboard pulp with a freeness of 400 ml, and was made into a three-layer cardboard liner paper using a multi-layer paper machine under the following papermaking conditions. The freeness was measured in accordance with JIS P8121 2012 using the following measuring device. Measuring device: Product name "Canadian Standard Freeness", Kumagai Riki Kogyo Co., Ltd., Product number "No. 2580-A".

[0130] - Papermaking conditions for product number "No. 1" > Sizing agent: Contains 0.3 parts by mass of "Sizepine N-830 (manufactured by Arakawa Chemical Industries, Ltd.)" for a total of 100 parts by mass of all pulp in the paper layers > Paper strength agent: Contains 0.5 parts by mass of "PT-1001 (manufactured by Arakawa Chemical Industries, Ltd.)" for a total of 100 parts by mass of all pulp in the paper layers > Aluminum sulfate: Contains 5 parts by mass of all pulp in the paper layers > Softwood kraft pulp: Contains 10% by mass of the pulp fiber in the surface layer. In addition, softwood kraft pulp accounted for 6% by mass of the total pulp in the paper layers. > Fine fiber content: Contains 36.7% of the pulp fiber that makes up the liner. The surface layer of the three layers of liner base paper was created under the above papermaking conditions. The papermaking conditions for the middle layer and the back layer of the three layers of the liner base paper are not limited to the above papermaking conditions.

[0131] The liner base paper of product number "No. 2" has a basis weight of 170 [g / m 2 The liner paper of product number "No. 3" was produced in the same manner as the liner paper of "No. 1", except that the basis weight was changed to 210 [g / m 2 The liner paper of product number "No. 4" was produced in the same manner as the liner paper of "No. 1", except that the basis weight was changed to 280 [g / m 2 ] was changed to "No. 1" and the same method was used to prepare the liner base paper.

[0132] Each of the liner base papers No. 5 to No. 15 was produced in the same manner as No. 2, except for the following: No. 5: Density was 0.7 [g / cm 3 ] No. 6: The amount of fine fibers was changed to 16.5 [%]. No. 7: The amount of fine fibers was changed to 19.8 [%]. No. 8: The amount of fine fibers was changed to 26.8 [%]. No. 9: The content of softwood kraft pulp in the surface layer pulp was changed to 20 [mass %], and the average fiber length was changed to 1.50 [mm].

[0133] No. 10: The amount of fine fibers was changed to 13.9%. No. 11: The amount of fine fibers was changed to 40.1%. No. 12: The density was changed to 0.5 g / cm. 3 No. 13: Density was changed to 0.9 [g / cm 3 No. 14: The amount of fine fibers was changed to 13.9 [%], and the density was changed to 0.5 [g / cm 3 No. 15: The content of softwood kraft pulp in the surface layer pulp was changed to 20 [mass%], the amount of fine fibers was changed to 40.1 [%], and the density was changed to 0.9 [g / cm 3 ] was changed to

[0134] In addition, when measuring the concentration of various chemicals contained in the liner paper, such as sizing agents and paper strength additives, the chemical concentration (relative to pulp weight ratio) was measured using a pyrolysis gas chromatograph mass spectrometer (pyrolysis device: PY-2020D manufactured by Frontier Labs, gas chromatograph mass spectrometer: 5973N manufactured by Agilent Technologies). Then, the liner paper to be analyzed was peeled from the core raw paper according to the following procedures F1 and F2, and after drying, the liner paper was pulverized in a pulverizer. Two samples of 200 to 300 μg of the pulverized material were measured using the pyrolysis gas chromatograph mass spectrometer.

[0135] In the pyrolysis gas chromatograph mass spectrometer, the peaks of the target drugs obtained when the calibration curve was created were used as a reference. The peak areas were extracted, and the peak areas were compared with the calibration curve to calculate the drug concentration of the target drug. This measurement was performed twice for each sample, and the average value was used as the drug concentration (weight ratio to pulp). The calibration curve samples were prepared by impregnating various drugs into filter paper (Advantec, circular qualitative filter paper, No. 2) and drying the paper so that the drug concentrations were 0.01%, 0.1%, 1%, 5%, and 10% by weight. Each calibration curve sample was pulverized, and 200-300 μg of the pulverized material was applied to the pyrolysis gas chromatograph mass spectrometer to create the calibration curve.

[0136] The density of the above product numbers "No. 5," "No. 12," and "No. 15" was changed by adjusting the nip pressure of the multi-layer paper machine. The amount of fine fibers and the average fiber length of the above product numbers "No. 6," "No. 11," "No. 14," and "No. 15" were adjusted using a fiber classifier (MAX-F700, manufactured by Aikawa Iron Works Co., Ltd.).

[0137] In each of Examples C1 to C11 and Comparative Examples C12 to C19, one of the following core raw papers, "No. 16" and "No. 17", was used for the core. No. 16: Basis weight 120 [g / m 2 ], density 0.65 [g / cm 3 ] [OND-EM120: manufactured by Oji Materia Co., Ltd.] No. 17: Basis weight 160 [g / m 2 ], density 0.65 [g / cm 3 For each of the above Examples C1 to C11 and Comparative Examples C12 to C19, the liner fiber information shown in Tables 8 to 10 was measured. Note that there is a possibility that the measurement values ​​of various parameters such as density, length-average fiber length, fine fibers, and basis weight may have a measurement error of approximately plus or minus 10%.

[0138]

[0139]

[0140]

[0141] "Liner fiber information" is information measured about the pulp fibers that make up the liner base paper, and includes three types: "Runkel ratio," "average fiber length," and "fine fiber content." The Runkel ratio is a parameter that indicates the shape of the pulp fiber, and is calculated as (Runkel ratio) = (twice the fiber wall thickness) / (fiber lumen diameter). A higher Runkel ratio indicates a more rigid fiber. The average fiber length is the average length (fiber length) of the pulp fibers that make up the liner. The fine fiber content is the percentage (%) of the amount of fine fibers contained relative to the total (100%) of the pulp fibers that make up the liner. Fine fibers are fine fibers with a fiber length of 0.0 mm or more and 0.2 mm or less.

[0142] The three types of "liner fiber information"—"Runkel ratio," "average fiber length," and "fine fiber content"—were measured using the following procedures F1 to F5. Procedure F1: The second-highest layer of cardboard material was cut into a 40-cm square, and this 40-cm square cardboard sheet was used for measurement. The cutout was located in the center of the cardboard sheet's width. The cardboard sheet was then immersed in ion-exchange water for 15 minutes and removed from the ion-exchange water. Procedure F2: The liner base paper (front liner and back liner) from the cardboard sheet removed in Procedure F1 was separated from the core base paper by manually peeling it off, taking care not to tear the liner base paper. Procedure F3: The liner base paper and core base paper separated in Procedure F2 were each immersed in ion-exchange water, adjusted to a concentration of 2%, and soaked for 24 hours. Step F4: The liner base paper and core base paper whose concentrations have been adjusted in Step F3 are each soaked for 24 hours, and then disintegrated for 20 minutes using a standard disintegrator (manufactured by Kumagai Riki Kogyo Co., Ltd.) to break down the pulp into fibers. Step F5: The slurry (pulp fibers) disintegrated in Step F4 was sampled, and the "Runkel ratio," "average fiber length," and "fine fiber content" were measured using the following fiber length measuring device. Fiber length measuring device: Part number FS-5 UHD base unit, manufactured by Valmet

[0143] Evaluation: For Examples C1 to C11 and Comparative Examples C12 to C19 whose "Runkel ratio," "average fiber length," and "fine fiber content" were measured as described above, the creasing property and texture were evaluated. "Creating property" is an evaluation criterion corresponding to the resistance to tearing at the fold where successive sheets of the measured cardboard material are folded back. "Texture" is an evaluation criterion corresponding to the uniformity of the distribution of pulp fibers that make up the liner of the measured cardboard material. The poorer the texture, the more non-uniform the fiber distribution, which tends to cause uneven strength in the liner and lead to creasing.

[0144] The crease resistance was evaluated by a load test following the following procedures G1 to G3. Procedure G1: The cardboard material to be measured was placed on a pallet, wrapped in stretch film, and left to stand for 24 hours under the following temperature and humidity conditions: Temperature: 10°C, Humidity: 10% Rh Procedure G2: After procedure G1, the cardboard material to be measured was impacted under the following conditions using the following vibrator: Vibrator: Product name "Multiaxial Vibration Tester", Model number "DS-3000-15L", manufactured by IMV Corporation Vibration force: 30 kN Vibration method: Random wave Frequency: 100 Hz Procedure G3: After procedures G1 and G2, the fold was visually inspected to determine whether any creases had occurred.

[0145] The creasing properties were evaluated according to the following criteria: ⊚: No creasing occurred at all on any of the folds after procedure G2. ◯: Crissing occurred on one or more folds after procedure G2. △: Crissing occurred on one or more folds after procedure G1. ×: Crissing occurred on one or more folds before procedure G1 (at the time of folding into an accordion fold). According to the above criteria, a rating of "◯" or higher was considered good, and a rating of "△" or lower was considered poor.

[0146] For the evaluation of "texture," the distribution of pulp fibers constituting the liner of the measured cardboard material was visually confirmed. The texture was evaluated according to the following criteria: ⊚: No unevenness in the pulp fibers. 〇: Unevenness in the pulp fibers (cloudy formation). ×: Aggregates of pulp fibers were observed. Based on the above criteria, "〇" or higher was evaluated as good, and "×" or lower was evaluated as poor.

[0147] In Examples C1 to C11, the density was 0.60 [g / cm 3 ] or more and 0.85 [g / cm 3 ] or less, the length average fiber length was 0.98 [mm] or more and 1.55 [mm] or less, the fine fiber content was 15 [%] or more and 38 [%] or less, and both the creasing property and the texture were rated as "Good" or better.

[0148] The density is 0.80 [g / cm 3Examples C9 to C11, in which the average fiber length was 1.10 mm or more and the fine fiber content was 18% or more, were evaluated as "Excellent" for creasing ability. Examples C1 to C7, in which the average fiber length was 0.98 mm or more and 1.05 mm or less, were evaluated as "Excellent" for texture.

[0149] On the other hand, the density is 0.60 [g / cm 3 ] or less than 0.85 [g / cm 3 In Comparative Examples C12 to C19, in which the average fiber length was greater than 0.98 mm or greater than 1.55 mm, or the amount of fine fibers was less than 15% or greater than 38% or less, at least the creasing property was evaluated as "△" or less.

[0150] In consideration of Comparative Examples C12 to C19, Examples C1 to C11 show that the density is 0.60 [g / cm 3 ] or more and 0.85 [g / cm 3 ] or less, the length-average fiber length is 0.98 [mm] or more and 1.55 [mm] or less, and the fine fiber content is 15 [%] or more and 38 [%] or less, it can be said that creases at the folds of the measured cardboard material are suppressed. 3

[0046] It can be said that when any one of the following is satisfied, creasing at the fold can be prevented. From Examples C1 to C7, it can be said that when the length-average fiber length is 0.99 [mm] or more and 1.00 [mm] or less, the texture is good.

[0151] From Comparative Examples C17 and C19, the density was 0.90 [g / cm 3 It is presumed that when the density is greater than 0.50 [g / cm], the gaps between the pulp fibers disappear, making it difficult for stress to escape when the liner is bent, and creasing is more likely to occur. In Comparative Example 19, the length-average fiber length is even larger than 1.55 [mm], so it is presumed that the liner becomes too hard, resulting in a poorer evaluation of creasing ability. From Comparative Examples C16 and C18, it is presumed that when the density is greater than 0.50 [g / cm], the gaps between the pulp fibers disappear, making it difficult for stress to escape when the liner is bent, making it more likely to crieve. 3], it is presumed that many gaps occur between the pulp fibers, the strength of the liner becomes insufficient, and creasing occurs easily.

[0152] From Comparative Examples C13 to C15, it is presumed that the average fiber length is less than 0.98 mm and the fine fiber content is greater than 38%, which results in a short average fiber length and a reduced proportion of long fibers, resulting in less entanglement of pulp fibers, resulting in insufficient liner strength and more susceptible to creasing. Furthermore, it is presumed that in Comparative Examples C13 to C15, the average fiber length is less than 0.98 mm and the fine fiber content is greater than 38%, which results in less noticeable differences between short and long fibers, resulting in good texture. In Comparative Example C19, the fine fiber content is greater than 38%, but the average fiber length is greater than 1.55 mm, which results in more clearly visible differences between short and long fibers, resulting in slightly poorer texture. From Comparative Example C12, it is presumed that the fine fiber content is less than 15%, which results in an increased proportion of long pulp fibers (long fibers), which results in more gaps between the long fibers, resulting in more susceptible to creasing.

[0153] [III. Modifications] The above-described embodiment is merely an example, and is not intended to exclude various modifications and application of techniques not explicitly described in this embodiment. Each configuration of this embodiment can be modified in various ways without departing from the spirit of the invention. Furthermore, it is possible to select and combine elements as needed.

[0154] For example, the cardboard material is not limited to the accordion-folded cardboard material 1, but may also be sheet-shaped cardboard material. The cardboard material may be single-sided cardboard with a liner on one side of the core. The device for folding cardboard into an accordion fold is not particularly limited. The above-mentioned problems I to IV may occur regardless of the structure of the folding device used for folding cardboard into an accordion fold. When the cardboard material is a material for a box-making system, it is preferable that additional processing such as intentionally formed slits or perforations is not applied to the fold, and it is preferable that the fold is a point where the cardboard material is folded 180° starting from a crease on the surface layer of the liner (e.g., with the crease inward). On the other hand, when the cardboard material is a material other than a box-making system, processing such as slits or perforations may be applied to the fold.

[0155] The uses of the accordion-folded cardboard material described above are not limited to use as a box-making material applied to a box-making system. The accordion-folded cardboard material has a structure in which multiple sheets are connected via folds, which is different from conventional single-sheet cardboard sheets. For example, when the accordion-folded cardboard material is unfolded, it can also be used as a web-like paper material with a large dimension in the extension direction.

[0156] Examples of uses for web-shaped paper materials include the following: Use as disaster supplies: By sticking it to windows, it can be used to prevent windows from breaking during typhoons, as a partition to protect privacy and reduce stress in evacuation shelters, and as a cushioning material or a mat to protect against the cold. Use at events: It can be used for creative projects such as signs for events and school events. Use as construction / moving materials: When doors, walls, and other items need to be temporarily protected at construction sites or moving sites, it can be used as a protective material (curing material) that can be stuck to the object. It can also be used as a protective material (packaging material) that can be wrapped around the object. In any of these uses, the structure in which multiple sheets are connected via folds has the advantage of improving work efficiency and ensuring the dimensions in the extension direction. [IV. Notes] Notes regarding the above embodiments are disclosed. [Appendix 1] A cardboard material using cardboard with a liner bonded to a core, wherein a measuring piece cut out from the liner has dynamic viscoelasticity measured in a tensile shear mode under a temperature condition of 25°C and a vibration condition of a frequency of 100 Hz, the dynamic viscoelasticity being within a predetermined range, the dynamic viscoelasticity being defined by the value of elastic modulus E' and tan δ, which is the ratio of loss modulus E'' to elastic modulus E', and the predetermined range being defined by the value of elastic modulus E' being 1.00 x 10 9 [MPa] or more and 8.00 × 10 9 [MPa] or less, and the tan δ is 2.50 × 10 -2 or more and 1.50 × 10 -1 [Appendix 2] The corrugated cardboard material characterized in that the elastic modulus E' is 3.00 x 10 or less. 9 [MPa] or less, and the tan δ is 7.00 × 10 -2 The corrugated cardboard material according to claim 1, characterized in that the elastic modulus E' is 4.00 x 10 or more. 9 [MPa] or more, and the tan δ is 4.00×10 -2[Appendix 4] The cardboard material according to any one of Appendices 1 to 3, wherein the freeness of the pulp used for the base paper forming the liner is 350 ml or more and 500 ml or less. [Appendix 5] The cardboard material according to any one of Appendices 1 to 4, wherein the cardboard is a double-sided cardboard in which the liner is bonded to both sides of the core. [Appendix 6] The cardboard material according to any one of Appendices 1 to 5, wherein the cardboard is an accordion-folded cardboard in which continuous strips of cardboard are alternately folded and stacked. [Appendix 7] A corrugated cardboard material using a cardboard with a liner bonded to a core, the cardboard being accordion-folded with continuous strips of the cardboard alternately folded and stacked, wherein the dynamic viscoelasticity of a test piece cut out from the liner, measured in a tensile shear mode under a temperature condition of 25°C and a vibration condition of a frequency of 100 Hz, is within a predetermined range, the dynamic viscoelasticity being defined by the value of elastic modulus E' and tanδ, which is the ratio of loss modulus E'' to elastic modulus E', and the predetermined range is defined as follows: the elastic modulus E' is 1.00 x 10 9 [MPa] or more and 3.00 × 10 9 [MPa] or less, and the tan δ is 7.00×10 -2 or more and 1.50 × 10 -1[Appendix 8] The cardboard material according to appendix 7, wherein the freeness of pulp used for the base paper forming the liner is 350 ml or more and 500 ml or less. [Appendix 9] The cardboard material according to appendix 7 or 8, wherein the cardboard is a double-sided cardboard having the liner bonded to both sides of the core. [Appendix 10] A cardboard material using cardboard having a liner laminated to a core, wherein the amount of sizing agent added to the liner is 0.2 parts by mass or more and 4.0 parts by mass or less, the amount of paper strength agent added to the liner is 0.1 parts by mass or more and 4.0 parts by mass or less, the pulp fibers constituting the liner have a length-average fiber length of 0.90 mm or more and 1.55 mm or less, and the amount of fine fibers having a fiber length of 0.0 mm or more and 0.2 mm or less among the pulp fibers constituting the liner is 23% or more and 48% or less. [Appendix 11] The cardboard material according to claim 10, wherein the amount of sizing agent added is 0.8 parts by mass or more. [Appendix 12] The cardboard material according to claim 10 or 11, wherein the amount of paper strength agent added is 1.0 parts by mass or more. [Appendix 13] The cardboard material according to any one of Appendices 10 to 12, characterized in that the length-average fiber length is 1.50 [mm] or more. [Appendix 14] The cardboard material according to any one of Appendices 10 to 13, characterized in that the content of fine fibers is 40 [%] or more. [Appendix 15] The cardboard material according to any one of Appendices 10 to 14, characterized in that the cardboard is double-sided cardboard in which the liner is bonded to both sides of the core. [Appendix 16] The cardboard material according to any one of Appendices 10 to 15, characterized in that the cardboard is accordion-folded in which continuous strips of cardboard are alternately folded and stacked. [Appendix 17] A cardboard material using cardboard in which a liner is bonded to a core, wherein the density of the liner is 0.60 [g / cm 3 ] or more and 0.85 [g / cm 3[Appendix 18] A corrugated cardboard material characterized in that the density is 0.80 [g / cm] or less, the length average fiber length of the pulp fibers constituting the liner is 0.98 [mm] or more and 1.55 [mm] or less, and the content of fine fibers having a fiber length of 0.0 [mm] or more and 0.2 [mm] or less among the pulp fibers constituting the liner is 15 [%] or more and 38 [%] or less. 3 [Appendix 19] The cardboard material according to Appendices 17, wherein the length-average fiber length is 0.98 mm or more and 1.05 mm or less, the length-average fiber length is 1.10 mm or more, and the content of fine fibers is 18% or more. [Appendix 20] The cardboard material according to any one of Appendices 17 to 19, wherein the cardboard is a double-sided cardboard having the liner bonded to both sides of the core. [Appendix 21] The cardboard material according to any one of Appendices 17 to 20, wherein the cardboard is an accordion-folded cardboard in which continuous strips of cardboard are alternately folded and stacked.

[0157] 1 Cardboard material 10 Fold (wave) 2 Sheet 20 Pair of sheets 21 First sheet 22 Second sheet 23 Third sheet 50 Folding device 50A Conveying part 50B Folding part 50C Stacking part F Fold L Auxiliary line L1 Vertical dimension (first dimension) L2 Horizontal dimension (second dimension) L3 Height dimension (third dimension)

Claims

1. A corrugated material using corrugated cardboard with a liner laminated to SMIC, wherein the dynamic viscoelasticity measured in a tensile shear mode under vibration conditions of a frequency of 100 [Hz] under a temperature condition of 25 [°C] for a measurement piece cut out from the liner is within a predetermined range, and the dynamic viscoelasticity is defined by a value of an elastic modulus E' and tanδ which is a ratio of a loss elastic modulus E'' to the elastic modulus E', and the predetermined range is such that the elastic modulus E' is 1.00×10 9 [MPa] or more and 8.00×10 9 [MPa] or less, and the tanδ is 2.50×10 -2 or more and 1.50×10 -1 or less. The corrugated material is characterized by this.

2. A corrugated material using corrugated cardboard with a liner laminated to SMIC, wherein the addition amount of the sizing agent added to the liner is 0.2 [parts by mass] or more and 4.0 [parts by mass] or less, the addition amount of the paper strength enhancer added to the liner is 0.1 [parts by mass] or more and 4.0 [parts by mass] or less, the average fiber length of the pulp fibers constituting the liner is 0.90 [mm] or more and 1.55 [mm] or less, and among the pulp fibers constituting the liner, the content of fine fibers having a fiber length of 0.0 [mm] or more and 0.2 [mm] or less is 23 [%] or more and 48 [%] or less. The corrugated material is characterized by this.

3. A corrugated material using corrugated cardboard with a liner laminated to SMIC, wherein the density of the liner is 0.60 [g / cm 3 or more and 0.85 [g / cm 3 or less, the average fiber length of the pulp fibers constituting the liner is 0.98 [mm] or more and 1.55 [mm] or less, and among the pulp fibers constituting the liner, the amount of fine fibers having a fiber length of 0.0 [mm] or more and 0.2 [mm] or less is 15 [%] or more and 38 [%] or less. A corrugated material characterized by this.