Circular polarizers and image display devices that utilize these polarizers.

VN10062528BActive Publication Date: 2026-10-26NITTO DENKO CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
VN1202306869
Authority / Receiving Office
VN · VN
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-03-04
Filing Date
2022-01-27
Publication Date
2026-10-26
Estimated Expiration
2042-01-27

AI Technical Summary

Technical Problem

Thin circularly polarizing plates used in organic EL displays face issues with retardation changes and reflected hue appearing red under high-temperature environments, due to their high moisture permeability and sensitivity to temperature fluctuations.

Method used

A circularly polarizing plate configuration with a polarizing plate, a first liquid crystal alignment solidified layer, a second liquid crystal alignment solidified layer, and a protective layer, where the protective layer has low moisture permeability and a glass transition temperature of 85°C or higher, suppressing changes in retardation and red discoloration.

Benefits of technology

The solution effectively maintains the optical properties of the circularly polarizing plate under high-temperature conditions, preventing changes in retardation and red discoloration, thus ensuring stable performance in thin display applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure VN1202306869_0
    Figure VN1202306869_0
Patent Text Reader

Abstract

The invention relates to a thin circular polarizing plate in which the change in slowness under high temperature conditions is suppressed and the phenomenon of the observed reddish reflection is also suppressed. The circular polarizing plate (100) consists in this order from the observer side: polarizing plate (10); first liquid crystal alignment fixative layer (20); second liquid crystal alignment fixative layer (30); and protective layer (40), which has a moisture permeability less than or equal to 920 (g / m2·24 hours).
Need to check novelty before this filing date? Find Prior Art

Description

Circularly polarizing plate and image display device using the same

[0001] The present invention relates to a circular polarizing plate and an image display device using the same.

[0002] With the spread of thin displays, displays equipped with organic EL panels have been proposed. Organic EL panels have a highly reflective metal layer, which can easily cause problems such as reflection of external light and glare of the background. Therefore, it is known that these problems can be prevented by providing a circular polarizer with a λ / 4 retardation film on the viewing side.

[0003] In recent years, as displays have become thinner, there has been a demand for thinner circular polarizers. However, such thin circular polarizers have problems such as changes in the phase difference of the retardation film and the reflection hue appearing red when exposed to a high-temperature environment for a long period of time.

[0004] Patent No. 3325560

[0005] The present invention has been made to solve the above-mentioned conventional problems, and its main object is to provide a thin circular polarizing plate in which the change in phase difference in a high-temperature environment is suppressed and the phenomenon in which the reflected hue is perceived as red is suppressed.

[0006] The circularly polarizing plate of the present invention comprises a polarizing plate, a first liquid crystal alignment solidified layer, a second liquid crystal alignment solidified layer, and a protective layer in this order from the viewing side, and the moisture permeability of the protective layer is 920 (g / m 224 hr or less. In one embodiment, the in-plane retardation Re(550) of the first liquid crystal alignment solidified layer is 100 nm to 180 nm, and satisfies the relationship Re(450)<Re(550)<Re(650). In one embodiment, the second liquid crystal alignment solidified layer exhibits refractive index characteristics of nz>nx=ny. In one embodiment, the protective layer contains an epoxy resin or an acrylic resin, and is a solidified or thermoset product of a coating film of an organic solvent solution of the resin. In one embodiment, the protective layer has a glass transition temperature of 85°C or higher, and the resin has a weight-average molecular weight Mw of 25,000 or higher. In one embodiment, the circularly polarizing plate of the present invention includes at least one other protective layer between the polarizing plate and the first liquid crystal alignment solidified layer. In one embodiment, the circularly polarizing plate of the present invention has a thickness of 100 μm or less. In another aspect of the present invention, there is provided an image display device, which includes the above-described circular polarizer.

[0007] According to an embodiment of the present invention, a polarizing plate, a first liquid crystal alignment solidified layer, a second liquid crystal alignment solidified layer, and a protective layer are provided in this order from the viewing side, and the moisture permeability of the protective layer is 920 (g / m 2 By keeping the time (time) to 24 hours or less, it is possible to obtain a thin circularly polarizing plate in which the change in retardation in a high-temperature environment is suppressed and the phenomenon in which the reflected hue is visually perceived as red is suppressed.

[0008] 1 is a schematic cross-sectional view of a circular polarizer according to one embodiment of the present invention.

[0009] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to these embodiments.

[0010] (Definition of Terms and Symbols) The definitions of terms and symbols used in this specification are as follows. (1) Refractive Index (nx, ny, nz) "nx" is the refractive index in the direction in which the in-plane refractive index is maximum (i.e., the slow axis direction), "ny" is the refractive index in the in-plane direction perpendicular to the slow axis (i.e., the fast axis direction), and "nz" is the refractive index in the thickness direction. (2) In-Plane Retardation (Re) "Re(λ)" is the in-plane retardation measured with light having a wavelength of λ nm at 23°C. For example, "Re(550)" is the in-plane retardation measured with light having a wavelength of 550 nm at 23°C. Re(λ) is calculated by the formula: Re(λ) = (nx - ny) × d, where d (nm) is the thickness of the layer (film). (3) Thickness Direction Retardation (Rth) "Rth(λ)" is the retardation in the thickness direction measured with light having a wavelength of λ nm at 23°C. For example, "Rth(550)" is the retardation in the thickness direction measured with light having a wavelength of 550 nm at 23°C. Rth(λ) is calculated by the formula: Rth(λ) = (nx - nz) x d, where d (nm) is the thickness of the layer (film). (4) Nz coefficient The Nz coefficient is calculated by Nz = Rth / Re. (5) Angle When an angle is mentioned in this specification, the angle includes both clockwise and counterclockwise angles relative to the reference direction. Therefore, for example, "45°" means ±45°.

[0011] A. Overall Configuration of Circular Polarizer FIG. 1 is a schematic cross-sectional view of a circular polarizer according to one embodiment of the present invention. The illustrated circular polarizer 100 includes a polarizer 10, a first liquid crystal alignment solidified layer 20, a second liquid crystal alignment solidified layer 30, and a protective layer 40, in this order from the viewing side. The polarizer 10 typically includes a polarizer 11 and a polarizer protective film 12 disposed on the viewing side of the polarizer 11. Depending on the purpose, another polarizer protective film (not shown) may be provided on the side opposite the viewing side of the polarizer 11. The first liquid crystal alignment solidified layer 20 is typically a retardation layer having a circular polarization function or an elliptically polarizing function.

[0012] In the embodiment of the present invention, the moisture permeability of the protective layer 40 is 920 (g / m 2When the moisture permeability of the protective layer is in this range, a change in retardation in a high-temperature environment is suppressed, and a thin circularly polarizing plate in which the phenomenon in which the reflected hue is visually perceived as red can be realized.

[0013] In one embodiment of the present invention, another protective layer may be provided between the polarizing plate and the first liquid crystal alignment solidified layer, and one or two protective layers may be provided between the polarizing plate and the first liquid crystal alignment solidified layer.

[0014] The circularly polarizing plate may further include other retardation layers, the optical properties (e.g., refractive index characteristics, in-plane retardation, Nz coefficient, photoelastic coefficient), thickness, arrangement position, etc. of which may be appropriately set depending on the purpose.

[0015] In practice, a pressure-sensitive adhesive layer 50 may be provided as the outermost layer on the surface of the protective layer 40 opposite the second liquid crystal alignment solidified layer 30. By providing the pressure-sensitive adhesive layer, the circular polarizer can be attached to an image display device (essentially, an image display panel). Furthermore, it is preferable that a release film is temporarily attached to the surface of the pressure-sensitive adhesive layer until the circular polarizer is used. Temporarily attaching the release film protects the pressure-sensitive adhesive layer and enables the circular polarizer to be formed into a roll.

[0016] The thickness of the circular polarizer is preferably 100 μm or less, more preferably 80 μm or less, even more preferably 70 μm or less, and particularly preferably 60 μm or less. The lower limit of the total thickness may be, for example, 40 μm. The thickness of the circular polarizer refers to the total thickness from the polarizer to the adhesive layer. According to an embodiment of the present invention, an extremely thin circular polarizer can be realized.

[0017] The circular polarizing plate may be in the form of a sheet or a long sheet. In this specification, the term "long sheet" refers to an elongated shape having a length that is sufficiently longer than its width, and includes, for example, an elongated shape having a length that is 10 times or more, preferably 20 times or more, the length of its width. A long circular polarizing plate can be wound into a roll.

[0018] The components of the circularly polarizing plate will be described in more detail below. Note that, since the pressure-sensitive adhesive layer may have a structure well known in the art, a detailed description of the structure of the pressure-sensitive adhesive layer will be omitted.

[0019] B. Polarizing Plate The polarizing plate includes a polarizer and a polarizer protective film disposed on at least one surface of the polarizer.

[0020] B-1. Polarizer Any appropriate polarizer can be used as the polarizer. For example, the resin film forming the polarizer may be a single-layer resin film or a laminate of two or more layers.

[0021] Specific examples of polarizers composed of a single-layer resin film include hydrophilic polymer films such as polyvinyl alcohol (PVA) films, partially formalized PVA films, and partially saponified ethylene-vinyl acetate copolymer films that have been dyed with iodine or a dichroic substance such as a dichroic dye and stretched, and polyene-based oriented films such as dehydrated PVA films and dehydrochlorinated polyvinyl chloride films. Preferably, a polarizer obtained by dyeing a PVA film with iodine and uniaxially stretching it is used because of its excellent optical properties.

[0022] The dyeing with iodine is carried out, for example, by immersing the PVA-based film in an aqueous iodine solution. The stretching ratio of the uniaxial stretching is preferably 3 to 7 times. The stretching may be carried out after the dyeing treatment or while dyeing. Alternatively, the PVA-based film may be stretched and then dyed. If necessary, the PVA-based film may be subjected to a swelling treatment, a crosslinking treatment, a washing treatment, a drying treatment, or the like. For example, by immersing the PVA-based film in water and washing it before dyeing, it is possible to wash away dirt and antiblocking agents from the surface of the PVA-based film and also to swell the PVA-based film, thereby preventing uneven dyeing and the like.

[0023] Specific examples of polarizers obtained using laminates include a laminate of a resin substrate and a PVA-based resin layer (PVA-based resin film) laminated on the resin substrate, or a polarizer obtained using a laminate of a resin substrate and a PVA-based resin layer coated on the resin substrate. A polarizer obtained using a laminate of a resin substrate and a PVA-based resin layer coated on the resin substrate can be produced, for example, by applying a PVA-based resin solution to the resin substrate and drying the solution to form a PVA-based resin layer on the resin substrate to obtain a laminate of the resin substrate and the PVA-based resin layer; and then stretching and dyeing the laminate to convert the PVA-based resin layer into a polarizer. In this embodiment, stretching typically involves immersing the laminate in an aqueous boric acid solution and stretching it. Furthermore, stretching may, if necessary, further involve in-air stretching of the laminate at an elevated temperature (e.g., 95°C or higher) before stretching in the aqueous boric acid solution. The obtained resin substrate / polarizer laminate may be used as is (i.e., the resin substrate may be used as a polarizer protective film), or the resin substrate may be peeled from the resin substrate / polarizer laminate and any appropriate polarizer protective film depending on the purpose may be laminated on the peeled surface. Details of such methods for producing polarizers are described in, for example, JP-A-2012-73580 (Japanese Patent No. 5414738) and Japanese Patent No. 6470455. The entire disclosures of these publications are incorporated herein by reference.

[0024] The thickness of the polarizer is preferably 25 μm or less, more preferably 1 μm to 22 μm, even more preferably 1 μm to 12 μm, and particularly preferably 3 μm to 12 μm. When the thickness of the polarizer is within this range, curling during heating can be well suppressed, and good appearance durability during heating can be obtained.

[0025] The polarizer preferably exhibits absorptive dichroism at any wavelength between 380 nm and 780 nm. The single transmittance of the polarizer is, as described above, 43.0% to 46.0%, preferably 44.5% to 46.0%. The degree of polarization of the polarizer is preferably 97.0% or more, more preferably 99.0% or more, and even more preferably 99.9% or more.

[0026] B-2. Polarizer Protective Film The polarizer protective film is formed of any appropriate film. Specific examples of materials that serve as the main component of the film include cellulose-based resins such as triacetyl cellulose (TAC), and transparent resins such as polyesters, polyvinyl alcohols, polycarbonates, polyamides, polyimides, polyethersulfones, polysulfones, polystyrenes, polynorbornenes, polyolefins, (meth)acrylics, and acetates. Other examples include thermosetting resins or ultraviolet-curing resins such as (meth)acrylics, urethanes, (meth)acrylic urethanes, epoxy resins, and silicone resins. Other examples include glassy polymers such as siloxane polymers. Polymer films described in JP 2001-343529 A (WO 01 / 37007) can also be used. Examples of materials that can be used for this film include a resin composition containing a thermoplastic resin having a substituted or unsubstituted imide group in its side chain and a thermoplastic resin having a substituted or unsubstituted phenyl group and a nitrile group in its side chain, such as a resin composition containing an alternating copolymer of isobutene and N-methylmaleimide and an acrylonitrile-styrene copolymer. The polymer film can be, for example, an extrusion molded product of the above resin composition.

[0027] As described below, the circular polarizing plate is typically disposed on the viewing side of an image display device, and the polarizer protective film 12 is typically disposed on the viewing side. Therefore, the polarizer protective film 12 may be subjected to a surface treatment such as a hard coat treatment, an anti-reflection treatment, an anti-sticking treatment, or an anti-glare treatment, as necessary. Furthermore / alternatively, the polarizer protective film may be subjected to a treatment to improve visibility when viewed through polarized sunglasses (typically, by imparting an (elliptical) circular polarization function or an ultra-high phase difference), as necessary. By performing such a treatment, excellent visibility can be achieved even when the display screen is viewed through polarized lenses such as polarized sunglasses. Therefore, the circular polarizing plate can also be suitably applied to image display devices that can be used outdoors.

[0028] In one embodiment, the another polarizer protective film is preferably optically isotropic. In this specification, "optically isotropic" means that the in-plane retardation Re(550) is 0 nm to 10 nm and the thickness direction retardation Rth(550) is -10 nm to +10 nm. Preferred materials constituting the another polarizer protective film include cyclic olefin resins (e.g., polynorbornene resins), cellulose resins (e.g., TAC), and acrylic resins.

[0029] The thickness of the polarizer protective film is preferably 10 μm to 50 μm, more preferably 10 μm to 30 μm. When a surface treatment is applied, the thickness of the outer polarizer protective film 12 includes the thickness of the surface treatment layer.

[0030] C. First Liquid Crystal Alignment Solidified Layer By using a liquid crystal compound, the difference between nx and ny in the first liquid crystal alignment solidified layer 20 can be significantly increased compared to non-liquid crystal materials, thereby significantly reducing the thickness of the first liquid crystal alignment solidified layer to obtain the desired in-plane retardation. As a result, a thinner circular polarizer can be achieved. In this specification, the term "liquid crystal alignment solidified layer" refers to a layer in which liquid crystal compounds are aligned in a predetermined direction within the layer and the alignment state is fixed. Note that the term "alignment solidified layer" encompasses the concept of an alignment solidified layer obtained by curing a liquid crystal monomer, as described below. In this embodiment, typically, rod-shaped liquid crystal compounds are aligned in the slow axis direction of the first liquid crystal alignment solidified layer (homogeneous alignment).

[0031] The first liquid crystal alignment solidified layer typically exhibits a refractive index characteristic of nx>ny=nz. The first liquid crystal alignment solidified layer is typically provided to impart anti-reflection properties to the polarizing plate and can function as a λ / 4 plate. In this case, the in-plane retardation Re(550) of the first liquid crystal alignment solidified layer is preferably 100 nm to 180 nm, more preferably 110 nm to 170 nm, and even more preferably 130 nm to 160 nm. Note that "ny=nz" here encompasses not only the case where ny and nz are completely equal, but also the case where they are substantially equal. Therefore, there may be cases where ny>nz or ny<nz, as long as the effects of the present invention are not impaired.

[0032] The Nz coefficient of the first liquid crystal alignment solidified layer is preferably 0.9 to 1.5, and more preferably 0.9 to 1.3. By satisfying such a relationship, when the obtained circularly polarizing plate is used in an image display device, an extremely excellent reflection hue can be achieved.

[0033] The first liquid crystal alignment solidified layer may exhibit a reverse dispersion wavelength characteristic in which the retardation value increases with the wavelength of the measurement light, a positive wavelength dispersion characteristic in which the retardation value decreases with the wavelength of the measurement light, or a flat wavelength dispersion characteristic in which the retardation value changes little with the wavelength of the measurement light. In one embodiment, the first liquid crystal alignment solidified layer preferably exhibits a reverse dispersion wavelength characteristic. That is, the first liquid crystal alignment solidified layer preferably satisfies the relationship Re(450)<Re(550)<Re(650). In this case, the Re(450) / Re(550) of the first liquid crystal alignment solidified layer is preferably 0.8 or more and less than 1, more preferably 0.8 or more and 0.95 or less. With this configuration, extremely excellent anti-reflection properties can be achieved.

[0034] The angle θ between the slow axis of the first liquid crystal alignment solidified layer and the absorption axis of the polarizer 11 is preferably 40° to 50°, more preferably 42° to 48°, and even more preferably about 45°. If the angle θ is in this range, by using the first liquid crystal alignment solidified layer as a λ / 4 plate as described above, a circular polarizer having excellent circular polarization properties (and consequently excellent antireflection properties) can be obtained.

[0035] The thickness of the first liquid crystal alignment solidified layer is preferably 0.5 μm to 7 μm, more preferably 1 μm to 5 μm. By using a liquid crystal compound, it is possible to achieve an in-plane retardation equivalent to that of a resin film with a thickness that is significantly thinner than that of a resin film.

[0036] Examples of liquid crystal compounds include liquid crystal compounds whose liquid crystal phase is a nematic phase (nematic liquid crystals). Examples of such liquid crystal compounds include liquid crystal polymers and liquid crystal monomers. The mechanism by which the liquid crystallinity of liquid crystal compounds is expressed may be either lyotropic or thermotropic. Liquid crystal polymers and liquid crystal monomers may be used alone or in combination.

[0037] When the liquid crystal compound is a liquid crystal monomer, the liquid crystal monomer is preferably a polymerizable monomer and a crosslinkable monomer. This is because the orientation state of the liquid crystal monomer can be fixed by polymerizing or crosslinking (i.e., curing) the liquid crystal monomer. After the liquid crystal monomer is aligned, for example, the alignment state can be fixed by polymerizing or crosslinking the liquid crystal monomers with each other. Here, a polymer is formed by polymerization, and a three-dimensional network structure is formed by crosslinking, but these are non-liquid crystals. Therefore, the formed first liquid crystal alignment solidified layer does not undergo, for example, a transition to a liquid crystal phase, a glass phase, or a crystalline phase due to temperature changes, which is typical of liquid crystal compounds. As a result, the first liquid crystal alignment solidified layer becomes a liquid crystal alignment solidified layer that is not affected by temperature changes and has excellent stability.

[0038] The temperature range in which the liquid crystal monomer exhibits liquid crystallinity varies depending on the type of the liquid crystal monomer. Specifically, the temperature range is preferably 40°C to 120°C, more preferably 50°C to 100°C, and most preferably 60°C to 90°C.

[0039] Any appropriate liquid crystal monomer can be used as the liquid crystal monomer. For example, polymerizable mesogen compounds described in JP-A-2002-533742 (WO 00 / 37585), EP 358208 (US 5,211,877), EP 66137 (US 4,388,453), WO 93 / 22397, EP 0,261,712, DE 19,504,224, DE 4,408,171, and GB 2,280,445 can be used. Specific examples of such polymerizable mesogen compounds include LC242 (product name) from BASF, E7 (product name) from Merck, and LC-Silicon-CC3767 (product name) from Wacker-Chem. As the liquid crystal monomer, for example, a nematic liquid crystal monomer is preferred.

[0040] The liquid crystal alignment solidified layer can be formed by performing an alignment treatment on the surface of a predetermined substrate, applying a coating liquid containing a liquid crystal compound to the surface to align the liquid crystal compound in a direction corresponding to the alignment treatment, and fixing the alignment state. In one embodiment, the substrate is any appropriate resin film, and the liquid crystal alignment solidified layer formed on the substrate can be transferred to the surface of an adjacent layer (e.g., a protective layer).

[0041] Any appropriate alignment treatment can be adopted as the alignment treatment. Specific examples include mechanical alignment treatment, physical alignment treatment, and chemical alignment treatment. Specific examples of mechanical alignment treatment include rubbing treatment and stretching treatment. Specific examples of physical alignment treatment include magnetic field alignment treatment and electric field alignment treatment. Specific examples of chemical alignment treatment include oblique deposition and photoalignment treatment. Any appropriate treatment conditions can be adopted for the various alignment treatments depending on the purpose.

[0042] The alignment of liquid crystal compounds is achieved by treating them at a temperature at which they exhibit a liquid crystal phase depending on the type of liquid crystal compound. By performing such temperature treatment, the liquid crystal compounds assume a liquid crystal state and are aligned in accordance with the alignment treatment direction on the substrate surface.

[0043] In one embodiment, the alignment state is fixed by cooling the liquid crystal compound aligned as described above. When the liquid crystal compound is a polymerizable monomer or a crosslinkable monomer, the alignment state is fixed by subjecting the liquid crystal compound aligned as described above to a polymerization treatment or a crosslinking treatment.

[0044] Specific examples of liquid crystal compounds and details of the method for forming the alignment solidified layer are described in JP-A-2006-163343, the disclosure of which is incorporated herein by reference.

[0045] D. Second Liquid Crystal Alignment Solidified Layer The second liquid crystal alignment solidified layer can be a so-called positive C plate, preferably exhibiting a refractive index characteristic of nz > nx = ny. Using a positive C plate as the second liquid crystal alignment solidified layer can effectively prevent reflections in oblique directions, enabling a wide viewing angle of the anti-reflection function. In this case, the thickness direction retardation Rth(550) of the second liquid crystal alignment solidified layer is preferably -50 nm to -300 nm, more preferably -70 nm to -250 nm, even more preferably -90 nm to -200 nm, and particularly preferably -100 nm to -180 nm. Here, "nx = ny" encompasses not only the case where nx and ny are strictly equal, but also the case where nx and ny are substantially equal. That is, the in-plane retardation Re(550) of the second liquid crystal alignment solidified layer can be less than 10 nm.

[0046] The second liquid crystal alignment solidified layer having a refractive index characteristic of nz > nx = ny can be formed from any appropriate material. The second liquid crystal alignment solidified layer is preferably composed of a film containing a liquid crystal material fixed in homeotropic alignment. The liquid crystal material (liquid crystal compound) that can be homeotropically aligned may be a liquid crystal monomer or a liquid crystal polymer. Specific examples of the liquid crystal compound and the method for forming the liquid crystal alignment solidified layer include those described in paragraphs

[0020] to

[0028] of JP 2002-333642 A (Patent No. 4174192). In this case, the thickness of the second liquid crystal alignment solidified layer is preferably 0.5 μm to 10 μm, more preferably 0.5 μm to 8 μm, and even more preferably 0.5 μm to 5 μm.

[0047] E. Protective Layer As described above, the protective layer is disposed between the second liquid crystal alignment solidified layer and the adhesive layer. Furthermore, the moisture permeability of the protective layer is 920 g / m 2 24 hours or less, preferably 900 g / m 2 24 hours or less, more preferably 880 g / m 2 The lower limit of the moisture permeability of the protective layer is, for example, 700 g / m 2 When the protective layer is disposed between the second liquid crystal alignment solidified layer and the pressure-sensitive adhesive layer and the moisture permeability of the protective layer is in this range, a change in retardation in a high-temperature environment is suppressed and a thin circularly polarizing plate in which the phenomenon of the reflected hue being perceived as red is suppressed can be obtained.

[0048] The protective layer is a solidified or thermoset product of a coating film of an organic solvent solution of a resin. This configuration allows for a very thin thickness (e.g., 10 μm or less). The thickness of the protective layer is preferably 0.01 μm to 5 μm, more preferably 0.02 μm to 3 μm, even more preferably 0.03 μm to 1 μm, and particularly preferably 0.04 μm to 0.6 μm. Furthermore, this configuration allows for the protective layer to be formed directly on an adjacent layer (e.g., a liquid crystal alignment solidified layer) (i.e., without an adhesive or pressure-sensitive adhesive layer interposed therebetween). According to an embodiment of the present invention, the polarizer, liquid crystal alignment solidified layer, and protective layer are very thin as described above, and an adhesive or pressure-sensitive adhesive layer for laminating the protective layer can be omitted, allowing for an extremely thin circular polarizer. Furthermore, such a protective layer has the advantage of excellent humidity durability due to its low moisture absorption and moisture permeability compared to solidified coating films of aqueous solutions or aqueous dispersions. As a result, a circular polarizing plate with excellent durability and capable of maintaining its optical properties even in a high-temperature, high-humidity environment can be realized. Furthermore, such a protective layer can suppress the adverse effects of ultraviolet irradiation on the polarizing plate (polarizer) compared to, for example, a cured product of an ultraviolet-curable resin. The protective layer is preferably a solidified product of a coating film of an organic solvent solution of the resin. The solidified product shrinks less during film formation compared to a cured product, and does not contain residual monomers, etc., so deterioration of the film itself is suppressed, and adverse effects on the polarizing plate (polarizer) caused by residual monomers, etc. can be suppressed.

[0049] Furthermore, the resin constituting the protective layer has a glass transition temperature (Tg) of 85°C or higher and a weight average molecular weight (Mw) of 25,000 or higher. When the Tg and Mw of the resin are within these ranges, a synergistic effect can be achieved by forming the protective layer from a solidified or thermoset product of a coating film of an organic solvent solution of the resin, thereby significantly suppressing migration of iodine in the polarizer to the image display cell despite the layer being very thin. The Tg of the resin is more preferably 90°C or higher, even more preferably 100°C or higher, particularly preferably 110°C or higher, and most preferably 120°C or higher. The upper limit of the Tg can be, for example, 200°C. The Mw of the resin is more preferably 30,000 or higher, even more preferably 35,000 or higher, and particularly preferably 40,000 or higher. The upper limit of the Mw can be, for example, 150,000.

[0050] Furthermore, the protective layer adjacent to the liquid crystal alignment solidified layer may further contain an isocyanate compound in addition to the resin. Examples of the isocyanate compound include tolylene diisocyanate, diphenylmethane diisocyanate, xylylene diisocyanate, and derivatives thereof (e.g., modified products and adducts). The isocyanate compounds may be used alone or in combination. The content ratio of the resin to the isocyanate compound (resin / isocyanate compound) is 95 / 5 to 10 / 90, as described above. The content ratio (resin / isocyanate compound) may be, for example, 95 / 5 to 50 / 50, or, for example, 90 / 10 to 60 / 40, or, for example, 85 / 15 to 70 / 30, or, for example, 85 / 15 to 75 / 25. The content ratio (resin / isocyanate compound) may also be, for example, 40 / 60 to 5 / 95, or for example, 30 / 70 to 5 / 95, or for example, 20 / 80 to 10 / 90. With such a configuration, peeling between the protective layer and the liquid crystal alignment solidified layer can be significantly suppressed.

[0051] The resin constituting the protective layer can be any suitable thermoplastic or thermosetting resin, as long as it can form a solidified or thermoset product of the coating film of the organic solvent solution and has the above-mentioned Tg and Mw. A thermoplastic resin is preferred. Examples of the thermoplastic resin include epoxy resins and acrylic resins. Epoxy resins and acrylic resins may also be used in combination. Representative examples of epoxy resins and acrylic resins that can be used in the protective layer are described below.

[0052] <Epoxy Resin> As the epoxy resin, an epoxy resin having an aromatic ring is preferably used. By using an epoxy resin having an aromatic ring as the epoxy resin, adhesion to a polarizer can be improved when a protective layer is disposed adjacent to the polarizer. Furthermore, when a pressure-sensitive adhesive layer is disposed adjacent to the protective layer, the anchoring force of the pressure-sensitive adhesive layer can be improved. Examples of epoxy resins having an aromatic ring include bisphenol-type epoxy resins such as bisphenol A-type epoxy resins, bisphenol F-type epoxy resins, and bisphenol S-type epoxy resins; novolac-type epoxy resins such as phenol novolac epoxy resins, cresol novolac epoxy resins, and hydroxybenzaldehyde phenol novolac epoxy resins; multifunctional epoxy resins such as glycidyl ether of tetrahydroxyphenylmethane, glycidyl ether of tetrahydroxybenzophenone, and epoxidized polyvinylphenol; naphthol-type epoxy resins, naphthalene-type epoxy resins, and biphenyl-type epoxy resins. Preferably, bisphenol A-type epoxy resins, biphenyl-type epoxy resins, and bisphenol F-type epoxy resins are used. Only one type of epoxy resin may be used, or two or more types may be used in combination.

[0053] <Acrylic Resin> Acrylic resins typically contain, as a main component, repeating units derived from (meth)acrylic acid ester monomers having a linear or branched structure. In this specification, (meth)acrylic refers to acrylic and / or methacrylic. Acrylic resins may contain repeating units derived from any appropriate copolymerizable monomer depending on the purpose. Examples of copolymerizable monomers (comonomers) include carboxyl group-containing monomers, hydroxyl group-containing monomers, amide group-containing monomers, aromatic ring-containing (meth)acrylates, and heterocycle-containing vinyl monomers. By appropriately setting the type, number, combination, and copolymerization ratio of the monomer units, an acrylic resin having the above-mentioned predetermined Tg and Mw can be obtained.

[0054] <Boron-Containing Acrylic Resin> In one embodiment, the acrylic resin includes a copolymer (hereinafter, may be referred to as a boron-containing acrylic resin) obtained by polymerizing a monomer mixture containing more than 50 parts by weight of a (meth)acrylic monomer and more than 0 part by weight and less than 50 parts by weight of a monomer represented by formula (1) (hereinafter, may be referred to as a copolymerization monomer): (wherein X represents a functional group containing at least one reactive group selected from the group consisting of a vinyl group, a (meth)acrylic group, a styryl group, a (meth)acrylamide group, a vinyl ether group, an epoxy group, an oxetane group, a hydroxyl group, an amino group, an aldehyde group, and a carboxyl group; R 1 and R 2 each independently represents a hydrogen atom, an optionally substituted aliphatic hydrocarbon group, an optionally substituted aryl group, or an optionally substituted heterocyclic group; R 1 and R 2 may be linked to each other to form a ring).

[0055] The boron-containing acrylic resin typically has a repeating unit represented by the following formula: By polymerizing a monomer mixture containing a copolymerizable monomer represented by formula (1) and a (meth)acrylic monomer, the boron-containing acrylic resin has a boron-containing substituent (e.g., a repeating unit k in the following formula) in its side chain. This can improve adhesion to a polarizer when the protective layer is disposed adjacent to the polarizer. The boron-containing substituent may be contained consecutively (i.e., in a block form) or randomly in the boron-containing acrylic resin. (In the formula, R 6 represents any functional group, and j and k represent integers of 1 or more).

[0056] <(Meth)acrylic Monomer> Any appropriate (meth)acrylic monomer can be used as the (meth)acrylic monomer, including, for example, a (meth)acrylic acid ester monomer having a linear or branched structure and a (meth)acrylic acid ester monomer having a cyclic structure.

[0057] Examples of (meth)acrylic acid ester monomers having a linear or branched structure include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, methyl 2-ethylhexyl (meth)acrylate, and 2-hydroxyethyl (meth)acrylate. Methyl (meth)acrylate is preferably used. The (meth)acrylic acid ester monomers may be used alone or in combination of two or more.

[0058] Examples of the (meth)acrylic acid ester monomer having a cyclic structure include cyclohexyl (meth)acrylate, benzyl (meth)acrylate, isobornyl (meth)acrylate, 1-adamantyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, dicyclopentanyl (meth)acrylate, biphenyl (meth)acrylate, o-biphenyloxyethyl (meth)acrylate, o-biphenyloxyethoxyethyl (meth)acrylate, m-biphenyloxyethyl acrylate, p-biphenyloxyethyl (meth)acrylate, o-biphenyloxyethyl (meth)acrylate, Examples of suitable monomers include biphenyl group-containing monomers such as 2-hydroxypropyl (meth)acrylate, p-biphenyloxy-2-hydroxypropyl (meth)acrylate, m-biphenyloxy-2-hydroxypropyl (meth)acrylate, N-(meth)acryloyloxyethyl-o-biphenylcarbamate, N-(meth)acryloyloxyethyl-p-biphenylcarbamate, N-(meth)acryloyloxyethyl-m-biphenylcarbamate, and o-phenylphenol glycidyl ether acrylate; terphenyl (meth)acrylate; and o-terphenyloxyethyl (meth)acrylate. 1-Adamantyl (meth)acrylate and dicyclopentanyl (meth)acrylate are preferred. The use of these monomers allows for the production of polymers with high glass transition temperatures. These monomers may be used alone or in combination of two or more.

[0059] Furthermore, instead of the (meth)acrylic acid ester monomer, a silsesquioxane compound having a (meth)acryloyl group may be used. By using a silsesquioxane compound, an acrylic polymer having a high glass transition temperature can be obtained. Silsesquioxane compounds having various skeletal structures, such as a cage structure, a ladder structure, and a random structure, are known. The silsesquioxane compound may have only one of these structures, or two or more of them. Only one silsesquioxane compound may be used, or two or more silsesquioxane compounds may be used in combination.

[0060] Examples of silsesquioxane compounds containing a (meth)acryloyl group include the MAC grade and AC grade of the SQ series manufactured by Toagosei Co., Ltd. MAC grades are silsesquioxane compounds containing a methacryloyl group, and specific examples include MAC-SQ TM-100, MAC-SQ SI-20, and MAC-SQ HDM. AC grades are silsesquioxane compounds containing an acryloyl group, and specific examples include AC-SQ TA-100 and AC-SQ SI-20.

[0061] The (meth)acrylic monomer is used in an amount of more than 50 parts by weight based on 100 parts by weight of the monomer mixture.

[0062] <Comonomer> As the copolymerizable monomer, a monomer represented by the above formula (1) is used. By using such a copolymerizable monomer, a boron-containing substituent is introduced into the side chain of the obtained polymer. Only one type of copolymerizable monomer may be used, or two or more types may be used in combination.

[0063] Examples of the aliphatic hydrocarbon group in the above formula (1) include a linear or branched alkyl group having 1 to 20 carbon atoms, which may have a substituent, a cyclic alkyl group having 3 to 20 carbon atoms, which may have a substituent, and an alkenyl group having 2 to 20 carbon atoms. Examples of the aryl group include a phenyl group having 6 to 20 carbon atoms, which may have a substituent, and a naphthyl group having 10 to 20 carbon atoms, which may have a substituent. Examples of the heterocyclic group include a 5-membered or 6-membered ring group containing at least one heteroatom, which may have a substituent. Note that R 1 and R 2 may be linked to each other to form a ring. 1 and R 2 is preferably a hydrogen atom or a linear or branched alkyl group having 1 to 3 carbon atoms, and more preferably a hydrogen atom.

[0064] The reactive group contained in the functional group represented by X is at least one selected from the group consisting of a vinyl group, a (meth)acrylic group, a styryl group, a (meth)acrylamide group, a vinyl ether group, an epoxy group, an oxetane group, a hydroxyl group, an amino group, an aldehyde group, and a carboxyl group. Preferably, the reactive group is a (meth)acrylic group and / or a (meth)acrylamide group. By containing these reactive groups, adhesion to a polarizer can be further improved when the protective layer is disposed adjacent to the polarizer.

[0065] In one embodiment, the functional group represented by X is preferably a functional group represented by Z-Y-, where Z represents a functional group containing at least one reactive group selected from the group consisting of a vinyl group, a (meth)acrylic group, a styryl group, a (meth)acrylamide group, a vinyl ether group, an epoxy group, an oxetane group, a hydroxyl group, an amino group, an aldehyde group, and a carboxyl group, and Y represents a phenylene group or an alkylene group.

[0066] Specifically, the following compounds can be used as the copolymerization monomer.

[0067] The copolymerization monomer is used in an amount of more than 0 part by weight and less than 50 parts by weight, preferably 0.01 part by weight or more and less than 50 parts by weight, more preferably 0.05 to 20 parts by weight, still more preferably 0.1 to 10 parts by weight, and particularly preferably 0.5 to 5 parts by weight, based on 100 parts by weight of the monomer mixture.

[0068] <Acrylic Resin Containing Lactone Ring or the Like> In another embodiment, the acrylic resin has a repeating unit containing a ring structure selected from a lactone ring unit, a glutaric anhydride unit, a glutarimide unit, a maleic anhydride unit, and a maleimide (N-substituted maleimide) unit. The repeating unit of the acrylic resin may contain only one type of repeating unit containing a ring structure, or may contain two or more types of repeating units containing a ring structure.

[0069] The lactone ring unit is preferably represented by the following general formula (2):

[0070] In general formula (2), R 2 , R 3 and R 4 are each independently a hydrogen atom or an organic residue having 1 to 20 carbon atoms. The organic residue may contain an oxygen atom. The acrylic resin may contain only a single lactone ring unit, and R 2 , R 3 and R 4 The acrylic resin having a lactone ring unit may contain a plurality of lactone ring units having different structures. Acrylic resins having a lactone ring unit are described in, for example, JP 2008-181078 A, the disclosure of which is incorporated herein by reference.

[0071] The glutarimide unit is preferably represented by the following general formula (3):

[0072]

[0073] In general formula (3), R 11 and R 12 each independently represents hydrogen or an alkyl group having 1 to 8 carbon atoms; R 13 represents an alkyl group having 1 to 18 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, or an aryl group having 6 to 10 carbon atoms. 11 and R 12 are each independently a hydrogen atom or a methyl group, and R 13 is hydrogen, a methyl group, a butyl group, or a cyclohexyl group. More preferably, R 11 is a methyl group, and R 12 is hydrogen, and R 13 is a methyl group. The acrylic resin may contain only a single glutarimide unit, and R 11 , R 12 and R 13Acrylic resins having glutarimide units may contain a plurality of glutarimide units having different structures. Examples of acrylic resins having glutarimide units are described in JP-A Nos. 2006-309033, 2006-317560, 2006-328334, 2006-337491 (Patent No. 4695439), 2006-337492, 2006-337493 (Patent No. 4686261), and 2006-337569, the disclosures of which are incorporated herein by reference. Note that the glutaric anhydride unit is represented by the R 13 The above description of the glutarimide unit applies, except that the nitrogen atom substituted with is an oxygen atom.

[0074] The structures of the maleic anhydride unit and the maleimide (N-substituted maleimide) unit are specified by their names, so a detailed explanation will be omitted.

[0075] The content of the repeating unit containing a ring structure in the acrylic resin is preferably 1 mol % to 50 mol %, more preferably 10 mol % to 40 mol %, and even more preferably 20 mol % to 30 mol %. The acrylic resin contains, as a main repeating unit, a repeating unit derived from the above (meth)acrylic monomer.

[0076] The protective layer can be formed by applying an organic solvent solution of the resin as described above to form a coating film, and then solidifying or thermally curing the coating film. Any appropriate organic solvent capable of dissolving or uniformly dispersing the acrylic resin can be used as the organic solvent. Specific examples of organic solvents include ethyl acetate, toluene, methyl ethyl ketone (MEK), methyl isobutyl ketone (MIBK), cyclopentanone, and cyclohexanone. The resin concentration in the solution is preferably 3 to 20 parts by weight per 100 parts by weight of the solvent. With such a resin concentration, a uniform coating film can be formed.

[0077] The solution may be applied to any suitable substrate or to an adjacent layer (e.g., a liquid crystal alignment solidified layer). When the solution is applied to a substrate, the solidified coating film (protective layer) formed on the substrate is transferred to the adjacent layer. When the solution is applied to an adjacent layer, the coating film is dried (solidified) to form a protective layer directly on the adjacent layer. Preferably, the solution is applied to the adjacent layer, and the protective layer is formed directly on the adjacent layer. With this configuration, the adhesive layer or pressure-sensitive adhesive layer required for transfer can be omitted, thereby making the circular polarizer even thinner. Any appropriate method can be used to apply the solution. Specific examples include roll coating, spin coating, wire bar coating, dip coating, die coating, curtain coating, spray coating, and knife coating (e.g., comma coating).

[0078] A protective layer can be formed by solidifying or thermally curing the coating film of the solution. The heating temperature for solidification or thermal curing is preferably 100°C or less, and more preferably 50°C to 70°C. If the heating temperature is within this range, adverse effects on the polarizer can be prevented. The heating time can vary depending on the heating temperature. The heating time can be, for example, 1 minute to 10 minutes.

[0079] The protective layer (essentially, the organic solvent solution of the resin) may contain any appropriate additive depending on the purpose. Specific examples of additives include ultraviolet absorbers; leveling agents; hindered phenol-based, phosphorus-based, sulfur-based antioxidants; stabilizers such as light stabilizers, weather stabilizers, and heat stabilizers; reinforcing materials such as glass fiber and carbon fiber; near-infrared absorbers; flame retardants such as tris(dibromopropyl)phosphate, triallyl phosphate, and antimony oxide; antistatic agents such as anionic, cationic, and nonionic surfactants; colorants such as inorganic pigments, organic pigments, and dyes; organic or inorganic fillers; resin modifiers; organic or inorganic fillers; plasticizers; lubricants; antistatic agents; and flame retardants. The type, number, combination, and amount of additives can be appropriately set depending on the purpose.

[0080] F. Image Display Device The circular polarizers described in the above sections A to E can be applied to image display devices. Accordingly, embodiments of the present invention encompass image display devices using such circular polarizers. Representative examples of image display devices include liquid crystal display devices and electroluminescence (EL) display devices (e.g., organic EL display devices, inorganic EL display devices). An image display device according to an embodiment of the present invention includes the circular polarizer described in the above sections A to E on its viewing side. The circular polarizer is laminated so that the liquid crystal alignment solidified layer faces the image display cell (e.g., liquid crystal cell, organic EL cell, inorganic EL cell) side (so that the polarizer faces the viewing side). In one embodiment, the image display device has a curved shape (essentially a curved display screen) and / or is bendable or foldable.

[0081] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The methods for measuring each property are as follows. Unless otherwise specified, "parts" and "%" in the examples and comparative examples are by weight.

[0082] (1) Thickness Thicknesses of 10 μm or less were measured using an interference film thickness meter (Otsuka Electronics Co., Ltd., product name "MCPD-3000"). Thicknesses exceeding 10 μm were measured using a digital micrometer (Anritsu Corporation, product name "KC-351C"). (2) Glass Transition Temperature (Tg) The glass transition temperature of the resin was measured using a differential scanning calorimeter DSC6220 manufactured by SII Nanotechnology Inc. Approximately 10 mg of the resin sample was placed in an aluminum pan manufactured by the same company, sealed, and heated from 30°C to 200°C at a heating rate of 20°C / min under a nitrogen gas flow of 50 mL / min. After holding the temperature for 3 minutes, the sample was cooled to 30°C at a rate of 20°C / min. After holding at 30°C for 3 minutes, the sample was again heated to 200°C at a rate of 20°C / min. From the DSC data obtained in the second temperature rise, the extrapolated glass transition onset temperature, which is the temperature at the intersection of a straight line extending the low-temperature baseline toward the high-temperature side and a tangent drawn at the point where the gradient of the curve of the stepwise change in the glass transition is maximum, was determined, and this was taken as the glass transition temperature (Tg). (3) Moisture permeability The protective layers obtained in the examples and comparative examples were applied to triacetyl cellulose (TAC) films, and the moisture permeability (g / m) was measured under test conditions of 40°C and 90% RH using "DELTAPERM" manufactured by Technolocks Co., Ltd. 224 hr). (4) Retardation Value A 50 mm x 50 mm sample was cut out from the retardation film obtained in the Examples and Comparative Examples to serve as a measurement sample. The in-plane retardation of the prepared measurement sample was measured using a retardation measurement device (product name "KOBRA21-ADH") manufactured by Oji Scientific Instruments Co., Ltd. The measurement wavelength for the in-plane retardation was 590 nm, and the measurement temperature was 23°C. (5) Change in Thermal Retardation Samples were prepared by bonding the circularly polarizing plates obtained in the Examples and Comparative Examples to glass via an adhesive layer, and the retardation was measured in the same manner as in the measurement of the retardation. After the measurement, the sample was placed in an environment of 85°C for 120 hours, and then the sample was removed and the retardation was measured again to determine the rate of change (%) of Re(590). Good: The absolute value of the rate of change in retardation (%) is less than 0.9%. Poor: The absolute value of the rate of change in retardation (%) is 0.9% or more. (6) Reddish Discoloration The circularly polarizing plates obtained in the examples and comparative examples were attached to a glass plate via an adhesive, and subjected to a heating test at 100°C for 120 hours, and the appearance before and after the heating test was visually observed. Good: No reddish discoloration was observed. Poor: Reddish discoloration was observed.

[0083] [Production Example 1: Preparation of boron-containing acrylic resin] 97.0 parts by weight of methyl methacrylate (MMA, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., trade name: methyl methacrylate monomer), 3.0 parts by weight of a monomer of general formula (1e), and 0.2 parts by weight of a polymerization initiator (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., trade name: 2,2'-azobis(isobutyronitrile)) were dissolved in 200 parts by weight of toluene. Subsequently, a polymerization reaction was carried out for 5.5 hours while heating to 70°C under a nitrogen atmosphere, to obtain Copolymer 1 (solid content concentration: 33% by weight). Copolymer 1 had a Tg of 110°C and a weight-average molecular weight of 80,000.

[0084] [Manufacturing Example 2: Preparation of Polarizing Plate A] 1. Preparation of Polarizer A A long, amorphous, isophthalic copolymerized polyethylene terephthalate film (thickness: 100 μm) with a water absorption rate of 0.75% and a Tg of approximately 75°C was used as the thermoplastic resin substrate. One side of the resin substrate was subjected to a corona treatment. A PVA-based resin (100 parts by weight of a 9:1 mixture of polyvinyl alcohol (degree of polymerization: 4200, degree of saponification: 99.2 mol%) and acetoacetyl-modified PVA (manufactured by Nippon Synthetic Chemical Industry Co., Ltd., trade name "GOHSEFIRMER Z410") was prepared. 13 parts by weight of potassium iodide was added to 100 parts by weight of the resulting PVA-based resin, and the resulting solution was dissolved in water to prepare an aqueous PVA solution (coating solution). The PVA-based resin layer was applied to the corona-treated surface of the resin substrate and dried at 60°C to form a 13 μm-thick PVA-based resin layer, producing a laminate. The resulting laminate was free-end uniaxially stretched 2.4 times in the longitudinal direction (machine direction) between rolls with different peripheral speeds in an oven at 130°C (in-air auxiliary stretching treatment). The laminate was then immersed in an insolubilizing bath (a boric acid aqueous solution obtained by blending 4 parts by weight of boric acid with 100 parts by weight of water) at a liquid temperature of 40°C for 30 seconds (insolubilization treatment). The laminate was then immersed in a dyeing bath (an iodine aqueous solution obtained by blending iodine and potassium iodide in a weight ratio of 1:7 with 100 parts by weight of water) at a liquid temperature of 30°C for 60 seconds while adjusting the concentration so that the single transmittance (Ts) of the final polarizer was 43.0% or higher (dyeing treatment). The laminate was then immersed in a crosslinking bath (a boric acid aqueous solution obtained by blending 3 parts by weight of potassium iodide and 5 parts by weight of boric acid with 100 parts by weight of water) at a liquid temperature of 40°C for 30 seconds (crosslinking treatment). The laminate was then immersed in a boric acid aqueous solution (boric acid concentration 4.0 wt%, potassium iodide concentration 5 wt%) at a liquid temperature of 70°C and uniaxially stretched in the longitudinal direction (longitudinal direction) between rolls with different peripheral speeds to a total stretch ratio of 5.5 (underwater stretching treatment). The laminate was then immersed in a cleaning bath (aqueous solution obtained by blending 4 parts by weight of potassium iodide with 100 parts by weight of water) at a liquid temperature of 20°C (washing treatment). Then, while drying in an oven maintained at 90°C, it was brought into contact with a SUS heated roll maintained at a surface temperature of 75°C for about 2 seconds (drying shrinkage treatment). The shrinkage rate of the laminate in the width direction due to the drying shrinkage treatment was 5.2%.In this manner, a polarizer A having a thickness of 5 μm was formed on the resin substrate.

[0085] 2. Preparation of Polarizing Plate A An HC-TAC film was attached as a polarizer protective film to the surface of the polarizer A obtained above (the surface opposite to the resin substrate) via a UV-curable adhesive. Specifically, the curable adhesive was applied so that the total thickness was 1.0 μm, and the films were attached using a roller. The adhesive was then cured by irradiation with UV light from the polarizer protective film side. The HC-TAC film was a triacetyl cellulose (TAC) film (thickness 25 μm) with a hard coat (HC) layer (thickness 7 μm), and the film was attached so that the TAC film faced the polarizer. The resin substrate was then peeled off to obtain a polarizing plate A having a configuration of HC layer / TAC film / adhesive layer / polarizer A.

[0086] [Production Example 3: Preparation of polarizing plate B] Polarizing plate B was obtained in the same manner as in Production Example 1, except that an HC-COP film was used as the polarizer protective film. The HC-COP film was a film in which a hard coat (HC) layer (thickness 2 μm) was formed on a cycloolefin (COP) film (manufactured by Zeon Corporation, product name "ZF12", thickness 25 μm).

[0087] [Production Example 4: Preparation of polarizing plate C] Polarizing plate C was obtained using polarizer A obtained in Production Example 1 in the same manner as in Production Example 1, except that an acrylic film (thickness: 20 μm) was used as the polarizer protective film.

[0088] [Production Example 5: Preparation of Polarizing Plate D] A long roll of a 30 μm-thick polyvinyl alcohol film (manufactured by Kuraray, product name "PE3000") was uniaxially stretched in the longitudinal direction by a roll stretching machine to 5.9 times its original length while simultaneously undergoing swelling, dyeing, crosslinking, and washing treatments, and finally drying treatment to obtain a 12 μm-thick polarizer D. An HC-TAC film similar to that in Production Example 1 was bonded to the polarizer D via a PVA-based adhesive as a polarizer protective film. Next, the resin substrate was peeled off, and a triacetyl cellulose (TAC) film (thickness 25 μm) was bonded to the released surface via a PVA-based adhesive to obtain polarizing plate D.

[0089] Production Example 6: Preparation of polarizing plate E Polarizing plate E was obtained in the same manner as in Production Example 1, except that a HC-TAC film was attached as a polarizer protective film using a PVA-based adhesive.

[0090] [Production Example 7: Preparation of First Liquid Crystal Alignment Solidified Layer and Second Liquid Crystal Alignment Solidified Layer] 1. Preparation of First Liquid Crystal Alignment Solidified Layer 55 parts of the compound represented by formula (I), 25 parts of the compound represented by formula (II), and 20 parts of the compound represented by formula (III) were added to 400 parts of cyclopentanone (CPN), heated to 60 ° C, and stirred to dissolve. After dissolution was confirmed, the mixture was returned to room temperature, and 3 parts of Irgacure 907 (manufactured by BASF Japan Ltd.), 0.2 parts of Megafac F-554 (manufactured by DIC Corporation), and 0.1 parts of p-methoxyphenol (MEHQ) were added and further stirred to obtain a solution. The solution was transparent and homogeneous. The resulting solution was filtered through a 0.20 μm membrane filter to obtain a polymerizable composition. Meanwhile, the polyimide solution for the alignment film was applied to a 0.7 mm thick glass substrate using a spin coating method, dried at 100 ° C for 10 minutes, and then baked at 200 ° C for 60 minutes to obtain a coating film. The resulting coating film was subjected to a rubbing treatment to form an alignment film. The rubbing treatment was performed using a commercially available rubbing device. The polymerizable composition obtained above was applied to a substrate (substantially an alignment film) by spin coating, and dried at 100°C for 2 minutes. After the resulting coating film was cooled to room temperature, it was irradiated with 30 mW / cm using a high-pressure mercury lamp. 2 The first liquid crystal alignment solidified layer was then irradiated with ultraviolet light at an intensity of 100 nm for 30 seconds to obtain a first liquid crystal alignment solidified layer. The in-plane retardation Re(550) of the first liquid crystal alignment solidified layer was 130 nm. The Re(450) / Re(550) of the first liquid crystal alignment solidified layer was 0.851, and the layer exhibited reverse dispersion wavelength characteristics.

[0091]

[0092] 2. Preparation of a Second Liquid Crystal Alignment Solidified Layer A liquid crystal coating solution was prepared by dissolving 20 parts by weight of a side-chain liquid crystal polymer represented by the following chemical formula (I) (the numbers 65 and 35 in the formula indicate the mole percentage of the monomer unit, conveniently expressed as a block polymer; weight-average molecular weight 5000), 80 parts by weight of a polymerizable liquid crystal exhibiting a nematic liquid crystal phase (manufactured by BASF: trade name Paliocolor LC242), and 5 parts by weight of a photopolymerization initiator (manufactured by Ciba Specialty Chemicals: trade name Irgacure 907) in 200 parts by weight of cyclopentanone. The coating solution was then applied to a substrate film (norbornene-based resin film: manufactured by Nippon Zeon Co., Ltd., trade name "Zeonex") using a bar coater, and the liquid crystal was aligned by heating and drying at 80°C for 4 minutes. The liquid crystal layer was irradiated with ultraviolet light to harden the liquid crystal layer, forming a second liquid crystal alignment solidified layer (thickness: 0.58 μm) on the substrate. This layer had an Re(550) of 0 nm and an Rth(550) of −80 nm, and exhibited refractive index characteristics of nz>nx=ny.

[0093]

[0094] [Example 1] The boron-containing acrylic resin prepared in Production Example 1 was applied to the first liquid crystal alignment solidified layer obtained in Production Example 7 to a dry thickness of 0.5 μm to form another protective layer. Next, the polarizing plate E obtained in Production Example 6 was laminated on the surface of the other protective layer via an acrylic adhesive (thickness 5 μm). Subsequently, the second liquid crystal alignment solidified layer obtained in Production Example 7 was transferred to the side of the first liquid crystal alignment solidified layer opposite the polarizer. The layers were bonded so that the angle between the absorption axis of the polarizer and the slow axis of the first liquid crystal alignment solidified layer was +45°. Each transfer (lamination) was performed via the UV-curable adhesive (thickness 1.0 μm) used in Production Example 2. In this way, a laminate having a configuration of HC layer / TAC film / adhesive layer / polarizer / acrylic adhesive layer / another protective layer / first liquid crystal alignment solidified layer / adhesive layer / second liquid crystal alignment solidified layer was prepared.

[0095] 15 parts (solids equivalent) of Copolymer 1 (boron-containing acrylic resin) obtained in Production Example 1 and 85 parts (solids equivalent) of a thermoplastic epoxy resin (manufactured by Mitsubishi Chemical Corporation, trade name "jER (registered trademark) YX6954BH30") were blended. The Tg of the resin blend was 125°C and the weight average molecular weight was 46,000. This mixture was dissolved in 80 parts of a mixed solvent of ethyl acetate / cyclopentanone (70 / 30) to obtain a resin solution (20%). This resin solution was applied to the surface of the second liquid crystal alignment solidified layer of the laminate obtained above using a wire bar, and the coating film was dried at 60°C for 5 minutes to form a protective layer (thickness 0.5 μm) composed of a solidified coating film of the organic solvent solution of the resin. Next, a pressure-sensitive adhesive layer (thickness 15 μm) was provided on the surface of the protective layer to obtain a circularly polarizing plate having a structure of HC layer / TAC film / adhesive layer / polarizer / acrylic pressure-sensitive adhesive layer / another protective layer / first liquid crystal alignment solidified layer / adhesive layer / second liquid crystal alignment solidified layer / protective layer / adhesive layer. The moisture permeability of the protective layer was 869.8 (g / m 2 The total thickness of the obtained circularly polarizing plate was 65 μm. The obtained circularly polarizing plate was subjected to the evaluations (4) to (6) above. The results are shown in Table 1.

[0096] Example 2 5 parts of an isocyanate compound (manufactured by Tosoh Corporation, "Coronate L": a trimethylolpropane adduct of tolylene diisocyanate) was added to 95 parts of a blend of 15 parts (solid content equivalent) of Copolymer 1 (boron-containing acrylic resin) obtained in Production Example 1 and 85 parts (solid content equivalent) of a thermoplastic epoxy resin (manufactured by Mitsubishi Chemical Corporation, trade name "jER (registered trademark) YX6954BH30"). The Tg of the resin blend was 23°C and the weight-average molecular weight was 50,000. Using this mixture, a circularly polarizing plate was obtained in the same manner as in Example 1. The moisture permeability of the protective layer was 901.7 (g / m 2 The total thickness of the obtained circularly polarizing plate was 65 μm. The obtained circularly polarizing plate was subjected to the evaluations (4) to (6) above. The results are shown in Table 1.

[0097] [Comparative Example 1] A circularly polarizing plate was obtained in the same manner as in Example 1, except that no protective layer was provided between the second liquid crystal alignment solidified layer and the pressure-sensitive adhesive layer. The total thickness of the obtained circularly polarizing plate was 64 μm. The obtained circularly polarizing plate was subjected to the evaluations (4) to (6) above. The results are shown in Table 1.

[0098] [Comparative Example 2] A circularly polarizing plate was obtained in the same manner as in Example 1, except that a trimethylolpropane / tolylene diisocyanate trimer adduct (manufactured by Nippon Polyurethane Industry Co., Ltd., product name "Coronate L") was used as the protective layer between the second liquid crystal alignment solidified layer and the adhesive layer. The moisture permeability of the protective layer was 944.6 (g / m 2 The total thickness of the obtained circularly polarizing plate was 66 μm. The obtained circularly polarizing plate was subjected to the evaluations (4) to (6) above. The results are shown in Table 1.

[0099] [Example 3] A circularly polarizing plate was obtained in the same manner as in Example 1, except that Polarizing Plate B was used as the polarizing plate. The total thickness of the obtained circularly polarizing plate was 61 μm. The obtained circularly polarizing plate was subjected to the evaluations (4) to (6) above. The results are shown in Table 1.

[0100] [Example 4] A circularly polarizing plate was obtained in the same manner as in Example 2, except that Polarizing Plate B was used as the polarizing plate. The total thickness of the obtained circularly polarizing plate was 61 μm. The obtained circularly polarizing plate was subjected to the evaluations (4) to (6) above. The results are shown in Table 1.

[0101] [Comparative Example 3] A circularly polarizing plate was obtained in the same manner as in Example 3, except that no protective layer was provided between the second liquid crystal alignment solidified layer and the pressure-sensitive adhesive layer. The total thickness of the obtained circularly polarizing plate was 60 μm. The obtained circularly polarizing plate was subjected to the evaluations (4) to (6) above. The results are shown in Table 1.

[0102] [Example 5] A circularly polarizing plate was obtained in the same manner as in Example 2, except that Polarizing Plate C was used as the polarizing plate. The total thickness of the obtained circularly polarizing plate was 54 μm. The obtained circularly polarizing plate was subjected to the evaluations (4) to (6) above. The results are shown in Table 1.

[0103] [Comparative Example 4] A circularly polarizing plate was obtained in the same manner as in Example 5, except that no protective layer was provided between the second liquid crystal alignment solidified layer and the pressure-sensitive adhesive layer. The total thickness of the obtained circularly polarizing plate was 53 μm. The obtained circularly polarizing plate was subjected to the evaluations (4) to (6) above. The results are shown in Table 1.

[0104] [Example 6] A circularly polarizing plate was obtained in the same manner as in Example 1, except that Polarizing Plate D was used as the polarizing plate. The total thickness of the obtained circularly polarizing plate was 96 μm. The obtained circularly polarizing plate was subjected to the evaluations (4) to (6) above. The results are shown in Table 1.

[0105] [Comparative Example 5] A circularly polarizing plate was obtained in the same manner as in Example 5, except that no protective layer was provided between the second liquid crystal alignment solidified layer and the pressure-sensitive adhesive layer. The total thickness of the obtained circularly polarizing plate was 95 μm. The obtained circularly polarizing plate was subjected to the evaluations (4) to (6) above. The results are shown in Table 1.

[0106] [Example 7] A circularly polarizing plate was obtained in the same manner as in Example 1, except that Polarizing Plate A was used as the polarizing plate. The total thickness of the obtained circularly polarizing plate was 65 μm. The obtained circularly polarizing plate was subjected to the evaluations (4) to (6) above. The results are shown in Table 1.

[0107] [Comparative Example 6] A circularly polarizing plate was obtained in the same manner as in Example 7, except that no protective layer was provided between the second liquid crystal alignment solidified layer and the pressure-sensitive adhesive layer. The total thickness of the obtained circularly polarizing plate was 64 μm. The obtained circularly polarizing plate was subjected to the evaluations (4) to (6) above. The results are shown in Table 1.

[0108] [Example 8] A circularly polarizing plate was obtained in the same manner as in Example 1, except that polarizing plate A was used and the copolymer obtained in Production Example 1 was not applied to the first liquid crystal alignment solidified layer. The total thickness of the obtained circularly polarizing plate was 65 μm. The obtained circularly polarizing plate was subjected to the evaluations (4) to (6) above. The results are shown in Table 1.

[0109] [Comparative Example 7] A circularly polarizing plate was obtained in the same manner as in Example 8, except that no protective layer was provided between the second liquid crystal alignment solidified layer and the pressure-sensitive adhesive layer. The total thickness of the obtained circularly polarizing plate was 64 μm. The obtained circularly polarizing plate was subjected to the evaluations (4) to (6) above. The results are shown in Table 1.

[0110]

[0111] [Evaluation] As is clear from Table 1, the circular polarizers of the examples of the present invention suppress the change in retardation under a heated environment. Furthermore, it can be seen that the circular polarizers of the examples of the present invention suppress the red discoloration of the circular polarizers.

[0112] The circular polarizer of the present invention is suitably used as a circular polarizer for liquid crystal displays, organic EL displays, and inorganic EL displays.

[0113] REFERENCE SIGNS LIST 10 Polarizing plate 11 Polarizer 12 Polarizer protective film 20 First liquid crystal alignment solidified layer 30 Second liquid crystal alignment solidified layer 40 Protective layer 50 Pressure-sensitive adhesive layer 100 Circularly polarizing plate

Claims

1. A polarizing plate, a first liquid crystal alignment solidified layer, a second liquid crystal alignment solidified layer, and a protective layer are provided in this order from the viewing side, and the moisture permeability of the protective layer is 920 (g / m 2 - 24 hr or less.

2. The circularly polarizing plate according to claim 1, wherein the in-plane retardation Re(550) of the first liquid crystal alignment solidified layer is 100 nm to 180 nm and satisfies the relationship Re(450)<Re(550)<Re(650).

3. The circular polarizer according to claim 1 or 2, wherein the second liquid crystal alignment solidified layer exhibits a refractive index characteristic of nz>nx=ny.

4. The circularly polarizing plate according to any one of claims 1 to 3, wherein the protective layer contains an epoxy resin or an acrylic resin, and is a solidified or heat-cured product of a coating film of a solution of the resin in an organic solvent.

5. The circularly polarizing plate according to claim 4, wherein the protective layer has a glass transition temperature of 85° C. or higher, and the resin has a weight average molecular weight Mw of 25,000 or higher.

6. The circular polarizer according to any one of claims 1 to 5, further comprising at least one additional protective layer between said polarizer and said first liquid crystal alignment solidified layer.

7. The circularly polarizing plate according to any one of claims 1 to 6, which has a thickness of 100 µm or less.

8. An image display device comprising the circular polarizing plate according to any one of claims 1 to 7.