Back-contact photovoltaic cells and methods for manufacturing these cells.

VN105032AActive Publication Date: 2024-08-26LONGI SOLAR TECHNOLOGY (TAIZHOU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
VN1202401844
Authority / Receiving Office
VN · VN
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-09-30
Filing Date
2022-05-11
Publication Date
2024-08-26
Estimated Expiration
2042-05-11

AI Technical Summary

Technical Problem

The existing back-contact cell manufacturing methods are complex, making it difficult to simplify the process while ensuring high photoelectric conversion efficiency.

Method used

The first doped layer and the second doped layer are formed with a staggered arrangement of the first doped region and the second doped region, with a stacked region and a third region in between, and the first doped layer and the second doped layer have opposite conductivity types. , protecting the first doping layer through the first protective layer, reducing the difficulty and cost of patterning processing, and improving the photoelectric conversion efficiency through the textured structure and polished surface.

Benefits of technology

The yield rate and production efficiency of the back contact battery are improved, the production cost is reduced, the photoelectric conversion efficiency and insulation performance are enhanced, and the production process is simplified.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure VN1202401844_0
    Figure VN1202401844_0
Patent Text Reader

Abstract

The invention relates to a reverse contact cell and a method for producing reverse contact cells, relating to the field of photovoltaic technology and used to simplify the process of producing reverse contact cells while ensuring high photovoltaic conversion efficiency.A reverse contact cell consists of a substrate, where the substrate has a first and second surface facing each other; on the first surface, there are a first and second doped region arranged in an alternating pattern; an overlap region and a third region are located between the first and second doped regions, with the overlap region close to the first doped region; the first doped layer is formed on the first doped region and the overlap region; the second doped layer is formed on the first doped layer and is located above the overlap region; the third doped layer is formed on the second doped region, where the conductivity of the third and second doped layers is opposite to the conductivity of the first doped layer; the first electrode is in electrical contact with the first doped layer and the second electrode is in electrical contact with the third doped layer. The manufacturing method described in the invention is used to produce the reverse contact cell.
Need to check novelty before this filing date? Find Prior Art

Description

Back contact battery and manufacturing method thereof

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to the Chinese patent disclosure with application number 202111162148.1, filed with the China Patent Office on September 30, 2021, entitled “A back contact battery and its manufacturing method”, the entire contents of which are incorporated by reference into this application. Technical Field

[0003] The present application relates to the field of photovoltaic technology, and in particular to a back-contact cell and a method for manufacturing the same. Background Art

[0004] Back-contact cells are cells with both the emitter and metal contacts on the back of the cell, leaving the front unobstructed by metal electrodes. Compared to cells with obstructed fronts, back-contact cells offer higher short-circuit current and photoelectric conversion efficiency, and are currently one of the technological advancements in achieving high-efficiency crystalline silicon cells.

[0005] The existing back contact cell manufacturing method is relatively complicated, so a simple method for manufacturing solar cells that ensures high efficiency is needed.

[0006] Overview

[0007] The purpose of the present application is to provide a back-contact cell and a method for manufacturing the same, so as to simplify the manufacturing process of the back-contact cell while ensuring high photoelectric conversion efficiency.

[0008] In a first aspect, the invention provides a back-contact battery, comprising: a substrate having a first surface and a second surface relative to each other. The first surface has first and second doping regions arranged alternately, and a stacked region and a third region between the first and second doping regions. The stacked region is adjacent to the first doping region. A first doping layer is formed on the first doping region and the stacked region. A second doping layer is formed on the first doping layer. The second doping layer is located only above the stacked region. The first doping layer and the second doping layer have opposite conductivity types. A third doping layer is formed on the second doping region, the third doping layer having opposite conductivity types to the first doping layer. And a first electrode and a second electrode. The first electrode is in electrical contact with the first doping layer. The second electrode is in electrical contact with the third doping layer.

[0009] When the above technical solution is adopted, the first surface of the substrate has a stacked region located between the first doping region and the second doping region and close to the first doping region, and the stacked region has a first doping layer and a second doping layer formed in sequence, and the first doping layer and the second doping layer have opposite conductivity types. Based on this, the second doping layer covers the first doping layer below it, protecting part of the surface of the first doping layer, avoiding the first doping layer in the stacked region from being damaged or introduced with impurities during subsequent process treatment, improving the yield and production efficiency of the back contact battery, and ensuring the collection of the first electrical carrier. In addition, the retained second doping layer reduces the processing area and difficulty in the graphic processing process, reduces production costs, and improves production capacity and production efficiency during mass production. In addition, the third region can separate the first doping layer on the first doping region from the third doping layer on the second doping region, which is conducive to ensuring the excellent positive and negative insulation performance of the battery.

[0010] In some possible implementations, a first protective layer is further included above the stacked region and between the first doped layer and the second doped layer.

[0011] When the above technical solution is adopted, on the one hand, in the process of gradually forming a back-contact battery, the first protective layer formed can protect the first doped layer in the subsequent graphic treatment, surface texturing treatment and cleaning process, so that the first doped layer will not be corroded or damaged. On the other hand, the first protective layer can completely separate the first doped layer and the second doped layer, thereby reducing the adverse effects of the second doped layer on the first doped layer in subsequent processes. For example, in the absence of the first protective layer, the first doped layer is in direct contact with the second doped layer. When at least one of the first doped layer and the second doped layer is a doped amorphous silicon layer that needs to be crystallized and converted into a doped polysilicon layer, due to the long crystallization time and the opposite conductivity type of the second doped layer and the first doped layer, the long crystallization time will cause the doping elements in the second doped layer to enter the first doped layer, causing damage to the first doped layer, and may even cause the conductivity type of the first doped layer to change, resulting in the battery being unable to generate electricity normally.

[0012] In some possible implementations, the first protective layer includes at least one of a dielectric layer and a mask layer. The dielectric layer and / or mask layer used in the first protective layer have relatively significant differences in physical or chemical properties from the first doped layer, thereby ensuring that the first protective layer can be effectively preserved when the first doped layer located in the second doped region and the third region is removed using an etching process or corrosion process.

[0013] In some possible implementations, the first protective layer includes one of a borosilicate glass layer and a phosphosilicate glass layer. In this case, the first protective layer can be formed by doping together with the first doping layer.

[0014] In some possible implementations, the surface of the third region has a suede structure. No electrodes are provided on the third region; instead, the third region can be textured to provide a suede structure. Because the suede structure has excellent light trapping and anti-reflection effects, it can also utilize light incident on the first surface, increasing the light absorption effect of the back-contact cell on the first surface. This allows the back-contact cell to absorb light energy from both sides, further utilizing light energy and improving the power generation efficiency of the back-contact cell.

[0015] In some possible implementations, the surface of the first doping region and / or the surface of the second doping region and / or the surface of the stacked region are polished surfaces.

[0016] When the above technical solution is adopted, the surfaces of the first doped region, the second doped region, and the stacked region can all be polished surfaces, so that light incident from the second surface and passing through the back contact cell is re-reflected, so that the light has the opportunity to be reused by the back contact cell, thereby improving the photoelectric conversion efficiency of the back contact cell. In addition, the polished surface has better flatness, and the subsequent formation of other layers on the polished surface will be more effective, which is conducive to reducing the generation of interface defects, thereby reducing the recombination of carriers caused by defects, and is conducive to improving the passivation performance of the back contact cell, thereby improving the photoelectric conversion efficiency of the back contact cell.

[0017] In some possible implementations, the present invention further includes a first interface passivation layer, a second interface passivation layer, and a third interface passivation layer. The first interface passivation layer is located between the substrate and the first doped layer. The second interface passivation layer is located between the second doped layer and the first protective layer. The third interface passivation layer is located between the substrate and the third doped layer. The first interface passivation layer, the second interface passivation layer, and the third interface passivation layer respectively passivate the interfaces of the substrate, the first protective layer, and the first doped layer, thereby reducing carrier recombination at the interfaces and ensuring carrier transmission efficiency.

[0018] In some possible implementations, the substrate is an n-type substrate, the first doped layer is a p-type doped layer, and the second and third doped layers are n-type doped layers; or, the substrate is a p-type substrate, the first doped layer is an n-type doped layer, and the second and third doped layers are p-type doped layers. When the substrate is an n-type substrate, the first doped layer is a p-type doped layer, and the second and third doped layers can both be phosphorus-doped n-type doped layers. In this case, because the heavily phosphorus-doped region has a greater solubility for metal impurities, the phosphorus in the second doped layer can provide phosphorus gettering passivation for the first doped layer, thereby improving battery efficiency.

[0019] In some possible implementations, the device further includes a first surface passivation layer. The first surface passivation layer covers the first doped layer, the second doped layer, the third doped layer, and the third region. The first surface passivation layer has a first opening at the interface between the first doped layer and the first doped layer. The first electrode is in electrical contact with the first doped layer through the first opening. The first surface passivation layer has a second opening at the interface between the first doped layer and the third doped layer. The second electrode is in electrical contact with the third doped layer through the second opening.

[0020] When the above technical solution is adopted, a first surface passivation layer is formed outside the first doped layer, the second doped layer, the third doped layer, and the third region. The first surface passivation layer can passivate the surface of the back-contact battery, passivating the dangling bonds in the first doped layer, the second doped layer, the third doped layer, and the third region, reducing the carrier recombination velocity on the first surface and improving the photoelectric conversion efficiency. The first electrode and the second electrode are electrically contacted with the first doped layer and the third doped layer through the first opening and the second opening, respectively, forming a local ohmic contact between the metal and the semiconductor. This reduces the contact area between the metal electrode and the first doped layer and the third doped layer, lowering the contact resistance, further reducing the carrier recombination velocity at the electrode surface, and improving the open circuit voltage.

[0021] In some possible implementations, the stacking area accounts for 5% to 95% of the area of ​​the first doping layer. Preferably, the stacking area accounts for 20% to 95% of the area of ​​the first doping layer. The larger the stacking area, the larger the area of ​​the first doping layer covered by the second doping layer, that is, the larger the area of ​​the protected first doping layer, which can better protect the first doping layer from corrosion or damage in subsequent process treatments. More preferably, the stacking area accounts for 40% to 75% of the area of ​​the first doping layer. The first protective layer, second doping layer, etc. above the stacking area should avoid contact with the electrode. In addition, if the stacking area is too large, there is a risk of leakage.

[0022] In a second aspect, the present application further provides a method for manufacturing a back-contact battery, comprising:

[0023] A substrate is provided, wherein the substrate has a first surface and a second surface opposite to each other, wherein the first surface has first doped regions and second doped regions arranged alternately, and a stacked region and a third region between the first doped regions and the second doped regions, wherein the stacked region is adjacent to the first doped region;

[0024] forming a first doped layer on the first surface of the substrate;

[0025] removing the first doping layer located in the second doping region and the third region;

[0026] forming a doped film layer on the first doped layer and the first surface;

[0027] removing the doped film layer located on the third region and the first doped region, so that the doped film layer located on the stacked region is the second doped layer, and the doped film layer located on the first surface is the third doped layer;

[0028] A first electrode is formed on the first doping layer, and a second electrode is formed on the third doping layer.

[0029] The beneficial effects of the method for manufacturing a back-contact battery provided by the second aspect or any possible implementation of the second aspect can be referred to the beneficial effects of the back-contact battery described in the first aspect or any possible implementation of the first aspect, and will not be repeated here.

[0030] In some possible implementations, the first doped layer located in the second doped region and the third region is removed by forming a first protective layer on the first doped region and the first doped layer in the stacked region, and removing the first doped layer and the first protective layer on the second doped region and the third region.

[0031] In some possible implementations, removing the doped film layer located on the third region and the first doped region specifically involves forming a second protective layer on the doped film layer located on the stacked region and the second doped region. Removing the doped film layer located on the third region and the first doped region. Removing the second protective layer.

[0032] In some possible implementations, before forming the first doping layer on the first surface of the substrate, the step is further included: forming a first interface passivation layer on the first surface of the substrate; in the step of removing the first doping layer located in the second doping region and the third region, the step is further included: removing the first interface passivation layer located in the second doping region and the third region; and / or, after removing the first doping layer located in the second doping region and the third region, and before forming the doping film layer on the first doping layer and the first surface, the step is further included: forming an interface passivation film layer on the first protective layer and the first surface; in the step of removing the doping film layer located in the third region and the first doping region, the step is further included: removing the interface passivation film layer located in the third region and the first doping region, so that the interface passivation film layer on the first protective layer in the stacking region is the second interface passivation layer, and the interface passivation film layer located on the first surface is the third interface passivation layer.

[0033] In some possible implementations, the first doping layer and the doping film layer are formed by an in-situ doping method or an ex-situ doping method.

[0034] In some possible implementations, after removing the doped film layer on the third region, the method further includes the step of texturing the third region.

[0035] In some possible implementations, forming a first electrode on the first doped layer and forming a second electrode on the third doped layer may be performed as follows: forming a first surface passivation layer on the first doped layer, the second doped layer, the third doped layer, and the third region; forming the first electrode on the first surface passivation layer located on the first doped layer; and forming the second electrode on the first surface passivation layer located on the third doped layer. The first electrode is in electrical contact with the first doped layer. The second electrode is in electrical contact with the third doped layer.

[0036] In some possible implementations, before forming a first surface passivation layer on the first doping layer, the second doping layer, the third doping layer and the third region, the step of performing a heat treatment process is further included, wherein the heat treatment process crystallizes at least a portion of the first doping layer and / or the second doping layer and / or the third doping layer.

[0037] In some possible implementations, the method of removing the first doped layer located in the second doped region and the third region and / or removing the doped film layer located in the third region and the first doped region is alkaline etching.

[0038] BRIEF DESCRIPTION OF THE DRAWINGS

[0039] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0040] Figures 1 to 3 are schematic structural diagrams of back-contact batteries provided in embodiments of the present application;

[0041] 4 to 13 are schematic diagrams of various stages of the back contact battery manufacturing process according to an embodiment of the present application;

[0042] FIG14 is a schematic diagram of a first surface of a back-contact battery provided in an embodiment of the present application;

[0043] FIG15 is a partial enlarged view of FIG14;

[0044] FIG16 is a schematic diagram of a first surface of a back-contact battery with continuous contact electrodes provided in an embodiment of the present application;

[0045] FIG17 is a partial schematic diagram of the first surface of a back-contact battery with a local contact electrode provided in an embodiment of the present application.

[0046] Reference numerals:

[0047] 10-substrate, 101-first doping region,

[0048] 102 - second doping region, 103 - third region,

[0049] 104-stacked region, 11-first doped layer,

[0050] 12- doped film layer, 121- second doped layer,

[0051] 122-third doping layer, 13-first surface passivation layer,

[0052] 130-first opening, 131-second opening,

[0053] 14-first interface passivation layer, 15-interface passivation film layer,

[0054] 151 - second interface passivation layer, 152 - third interface passivation layer,

[0055] 16-first protective layer, 17-second protective layer,

[0056] 20-first electrode, 21-second electrode,

[0057] 201-first electrode main electrode, 202-first electrode secondary gate line,

[0058] 211 - second electrode main electrode, 212 - second electrode auxiliary gate line,

[0059] 203-connecting electrodes, 204-fine grid lines,

[0060] 18-second surface passivation layer, 205-local contact point.

[0061] Detailed description

[0062] In order to make the technical problems, technical solutions and beneficial effects to be solved by this application more clearly understood, this application is further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain this application and are not intended to limit this application.

[0063] It should be noted that when an element is referred to as being “fixed on” or “disposed on” another element, it may be directly on the other element or indirectly on the other element. When an element is referred to as being “connected to” another element, it may be directly connected to the other element or indirectly connected to the other element.

[0064] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of this application, "multiple" means two or more, unless otherwise clearly and specifically defined. "Several" means one or more, unless otherwise clearly and specifically defined.

[0065] In the description of this application, it should be understood that the terms "up", "down", "front", "back", "left", "right", etc., indicating directions or positional relationships, are based on the directions or positional relationships shown in the accompanying drawings. They are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific direction, be constructed and operated in a specific direction. Therefore, they should not be understood as limitations on this application.

[0066] In the description of this application, it should be noted that, unless otherwise expressly specified or limited, the terms "installed," "connected," and "connected" should be understood in a broad sense. For example, they can refer to fixed connections, detachable connections, or integral connections; they can refer to mechanical connections or electrical connections; they can refer to direct connections or indirect connections through an intermediate medium; they can refer to internal communication between two components or the interaction between two components. Those skilled in the art will understand the specific meanings of the above terms in this application based on the specific circumstances.

[0067] Solar cells are becoming increasingly popular as a new energy alternative. They convert sunlight into electricity. They utilize the photovoltaic principle to generate charge carriers, which are then extracted using electrodes, facilitating efficient use of the electrical energy.

[0068] Interdigitated back contact cells, also known as IBC cells. IBC stands for Interdigitated back contact (Chinese name: Interdigitated back contact). The biggest feature of IBC cells is that the emitter and metal contact are both on the back of the cell. There is no metal electrode blocking the front, so it has a higher short-circuit current Isc. At the same time, the back can allow for wider metal grid lines to reduce the series resistance Rs and thus increase the fill factor FF. Moreover, this type of cell with no obstruction on the front not only has high conversion efficiency, but also looks more beautiful. At the same time, the full back electrode component is easier to assemble. IBC cells are one of the current technical directions for achieving high-efficiency crystalline silicon cells.

[0069] However, the manufacturing method of IBC cells is relatively complex and usually requires multiple steps of patterning to complete the preparation. A simple method for manufacturing solar cells that can ensure high efficiency is needed.

[0070] In order to solve the above technical problems and simplify the manufacturing process of the back-contact cell while ensuring high photoelectric conversion efficiency, an embodiment of the present application provides a back-contact cell.

[0071] As shown in Figures 1 to 3 and Figures 14 and 15 , the back-contact cell provided in an embodiment of the present application includes: a substrate 10 having opposing first and second surfaces. The first surface has alternating first and second doped regions 101 and 102, as well as a stacked region 104 and a third region 103 between the first and second doped regions 101 and 102. The stacked region 104 is adjacent to the first doped region 101. A first doped layer 11 is formed on the first doped region 101 and the stacked region 104. A second doped layer 121 is formed on the first doped layer 11. The second doped layer 121 is located only above the stacked region 104. The first doped layer 11 and the second doped layer 121 have opposite conductivity types. A third doped layer 122 is formed on the second doped region 102, and the third doped layer 122 has opposite conductivity types to the first doped layer 11. Furthermore, a first electrode 20 and a second electrode 21 are provided. The first electrode 20 is in electrical contact with the first doped layer 11. The second electrode 21 is in electrical contact with the third doped layer 122.

[0072] As can be seen from the structure of the back-contact battery described above, the first surface of the substrate 10 has a stacked region 104 located between the first doped region 101 and the second doped region 102 and adjacent to the first doped region 101. The stacked region 104 has a first doped layer 11 and a second doped layer 121 formed sequentially thereon, with the first doped layer 11 and the second doped layer 121 having opposite conductivity types. Therefore, the second doped layer 121 covers the first doped layer 11 below it, protecting a portion of the surface of the first doped layer 11 and preventing the first doped layer 11 in the stacked region 104 from being damaged or introduced with impurities during subsequent processing. This improves the yield and production efficiency of the back-contact battery while also ensuring the collection of first electrical carriers. Furthermore, the retained second doped layer 121 reduces the processing area and difficulty in the patterning process, lowering production costs and improving production capacity and efficiency during mass production. Furthermore, the third region 103 can separate the first doped layer 11 on the first doped region 101 from the third doped layer 122 on the second doped region 102, which helps ensure excellent insulation performance between the positive and negative electrodes of the battery.

[0073] In some examples, as shown in Figures 1 to 3, the width of the third region 103 ranges from 10μm to 100μm along the direction in which the first doping region 101 and the second doping region 102 are staggered. A third region 103 that is too wide may cause the effective area of ​​the back contact battery to be wasted, and effective carriers may be difficult to collect, thereby reducing battery performance. The third region 103 is arranged between the first doping region 101 and the second doping region 102, so that the first doping region 101 and the second doping region 102 are separated from each other at the boundary, eliminating the insulator design between the positive electrode and the negative electrode in the prior art, which can reduce the production process flow and reduce spatial complexity. Such a structure will not have the coexistence of positive and negative electrodes in the vertical direction, avoiding the occurrence of leakage in the back contact battery; it can also improve the reliability performance of the battery in later products and reduce the difficulty of the production process of the back contact battery.

[0074] For example, as shown in FIG. 1 to FIG. 3 , the width of the third region 103 may be 10 μm, 100 μm, or 60 μm.

[0075] Among them, the substrate 10 is a semiconductor substrate 10. The material of the substrate 10 can be selected from materials such as silicon (Si) or germanium (Ge) or materials such as gallium arsenide (GaAs). Obviously, in terms of conductivity type, the substrate 10 can be an intrinsic conductive substrate 10, an n-type conductive substrate 10, or a p-type conductive substrate 10. Preferably, the substrate 10 is a p-type conductive substrate 10 or an n-type conductive substrate 10. Compared with the intrinsic conductive substrate 10, the p-type conductive substrate 10 or the n-type conductive substrate 10 has better conductivity, so that the final back-contact battery has a lower bulk resistivity, thereby improving the efficiency of the back-contact battery.

[0076] Exemplarily, the substrate 10 is an n-type silicon substrate 10. Compared with the p-type conductive substrate 10, the n-type conductive substrate 10 has advantages such as long minority carrier lifetime, no light decay, and good weak light performance.

[0077] The first doping layer 11, the second doping layer 121 and the third doping layer 122 are also semiconductor doping layers. In terms of the internal arrangement of the material, the first doping layer 11, the second doping layer 121 and the third doping layer 122 can be amorphous, microcrystalline, single crystal, nanocrystalline or polycrystalline. In terms of specific materials, the materials of the first doping layer 11, the second doping layer 121 and the third doping layer 122 can be silicon (Si), germanium (Ge), silicon carbide (SiC x ) or gallium arsenide (GaAs), etc. In terms of conductivity type, the first doping layer 11, the second doping layer 121 and the third doping layer 122 can be n-type doping layers or p-type doping layers.

[0078] In some examples, when the substrate 10 is an n-type substrate 10, the first doping layer 11 can be a p-type doping layer, and the second doping layer 121 and the third doping layer 122 can be n-type doping layers; or, when the substrate 10 is a p-type substrate 10, the first doping layer 11 can be an n-type doping layer, and the second doping layer 121 and the third doping layer 122 can be p-type doping layers.

[0079] For example, as shown in Figures 1 to 3, substrate 10 is an n-type silicon substrate 10, first doped layer 11 is a boron-doped p-type doped layer, and second doped layer 121 and third doped layer 122 are both phosphorus-doped n-type doped layers. In this case, because the heavily phosphorus-doped region has a greater solubility for metal impurities, the phosphorus in second doped layer 121 can provide phosphorus gettering passivation for first doped layer 11, thereby improving cell efficiency.

[0080] In practical applications, when the first doped layer 11 on the first doped region 101 is a p-type doped layer, the entire stack on the stack region 104 actually also functions as a p-type doped layer. That is, the second doped layer 121 above the first doped layer 11 on the stack region 104 is not conductive. Only the first doped region 101 and the first doped layer 11 on the stack region 104 function to transport carriers. The carriers on the first doped layer 11 are then extracted through the first electrode 20 that is in electrical contact with the first doped layer 11. The p-type region on the entire cell can also be considered to be the combination of the first doped region 101 and the stack region 104.

[0081] As some possible implementations, as shown in FIG. 1 to FIG. 3 , a first protective layer 16 is further included above the stacked region 104 and between the first doping layer 11 and the second doping layer 121 .

[0082] Based on this, on the one hand, during the process of gradually forming a back-contact cell, the formed first protective layer 16 can protect the first doped layer 11 during the subsequent patterning, surface texturing, and cleaning processes, preventing the first doped layer 11 from being corroded or damaged. On the other hand, the first protective layer 16 can completely separate the first doped layer 11 from the second doped layer 121, thereby reducing the adverse effects of the second doped layer 121 on the first doped layer 11 in subsequent processes. For example, in the absence of the first protective layer 16, when the first doped layer 11 is in direct contact with the second doped layer 121, when at least one of the first doped layer 11 and the second doped layer 121 is a doped amorphous silicon layer that needs to be crystallized and converted into a doped polycrystalline silicon layer, due to the long crystallization time and the opposite conductivity type of the second doped layer 121 and the first doped layer 11, the long crystallization time may cause the doping elements in the second doped layer 121 to enter the first doped layer 11, causing damage to the first doped layer 11, and may even cause the conductivity type of the first doped layer 11 to change, resulting in the cell being unable to generate electricity normally. For example, in the absence of the first protective layer 16, when the first doped layer 11 is in direct contact with the second doped layer 121, when the first doped layer 11 is a P-type polycrystalline silicon layer doped with boron, and the second doped layer 121 is an N-type amorphous silicon layer doped with phosphorus, and the second doped layer 121 needs to be crystallized and transformed into an N-type polycrystalline silicon layer, during the crystallization process, the phosphorus element contained in the second doped layer 121 may enter the first doped layer 11 and damage the first doped layer 11; excessive phosphorus entering may also cause the first doped layer 11 to change from P-type to N-type, which is the same conductive type as the substrate 10, causing the battery to be unable to generate electricity.

[0083] In some examples, the first protective layer 16 includes at least one of a dielectric layer and a mask layer. The dielectric layer and / or mask layer used in the first protective layer 16 has relatively significant differences in physical or chemical properties from the first doped layer 11, so as to ensure that the first protective layer 16 can be effectively retained when the first doped layer 11 located in the second doped region 102 and the third region 103 is removed using an etching process or corrosion process.

[0084] In practical applications, the material of the first protective layer 16 can be one or more of oxides, nitrides, carbides, and hydrogenated amorphous silicon, wherein oxides include one or more of silicon oxide, silicon oxynitride, aluminum oxide, titanium oxide, hafnium dioxide (HfO2), gallium oxide (Ga2O3), tantalum pentoxide (Ta2O5), niobium pentoxide (Nb2O5), etc.; nitrides include one or more of silicon nitride, silicon carbonitride, aluminum nitride, titanium nitride (TiN), titanium carbonitride (TiCN), etc.; and carbides include silicon carbide (SiC).

[0085] For example, when an alkali etching process is used to remove the first doping layer 11 located in the second doping region 102 and the third region 103, a dielectric layer that does not react with the alkali used can be selected as the first protective layer 16. On the contrary, the first doping layer 11 will react with the selected alkali. Based on this, during the patterning process of the first doping layer 11, the first doping layer 11 located in the second doping region 102 and the third region 103 is removed, and the first doping layer 11 covered by the first protective layer 16 is completely retained. For example, silicon oxide, silicon nitride or silicon carbide (SiC x ) as the dielectric layer. When an oxide is selected as the dielectric layer, the dielectric layer can be formed by a thermal growth process, that is, in an oxidizing atmosphere (such as air, oxygen, etc.), a heating method is used to form an oxide dielectric layer on the surface of the first doped layer 11.

[0086] For another example, when a laser etching process is used to remove the first doping layer 11 located in the second doping region 102 and the third region 103, a mask layer resistant to laser ablation can be selected as the first protective layer 16. On the contrary, the first doping layer 11 will be ablated by the laser. Based on this, in the process of patterning the first doping layer 11, the first doping layer 11 located in the second doping region 102 and the third region 103 is removed, and the first doping layer 11 covered by the first protective layer 16 is completely retained. For example, the mask layer used can be a mask that can be photolithographically developed or laser patterned, a printable colloid mask, a silicon nitride (SiN x ), silicon oxide (SiO x ) or silicon carbide (SiC) and other materials.

[0087] In addition, when the first protective layer 16 is a stacked structure of a dielectric layer and a mask layer, preferably, the dielectric layer should be close to the first doping layer 11 to ensure the passivation effect of the first doping layer 11; the mask layer should be away from the first doping layer 11 due to the large amount of impurities to avoid contamination of the first doping layer 11.

[0088] In some examples, the first protective layer 16 includes one of a borosilicate glass (BSG) layer and a phosphosilicate glass (PSG) layer. In this case, the first protective layer 16 can be doped together with the first doped layer 11, eliminating the need to form the first protective layer 16 separately. When the second doped layer 121 located on the first protective layer 16 also needs to be doped, the BSG or PSG located between the first doped layer 11 and the second doped layer 121 can block the diffusion of phosphorus or boron, providing isolation and better protection for the first doped layer 11.

[0089] In practical applications, the material of the first protective layer 16 can be silicon oxide. Due to the property that silicon oxide does not react with alkali, when alkali is used for etching in subsequent processes, silicon oxide can better protect the integrity of the first doped layer 11. In addition, silicon oxide has a good interface passivation effect, which can passivate the dangling bonds on the surface of the first doped layer 11, inhibit the recombination of carriers on the surface of the first doped layer 11, and thus improve the photoelectric conversion efficiency of the battery. When the material of the first protective layer 16 is silicon oxide, the thickness of the first protective layer 16 ranges from 20nm to 100nm. In order to better protect the first doped layer 11 during etching or cleaning, the first protective layer 16 can be thicker.

[0090] As some possible implementations, as shown in Figures 2 and 3 , the surface of the third region 103 has a suede structure. While no electrodes are provided on the third region 103, the third region 103 can be texturized to provide a suede structure. Because the suede structure has excellent light trapping and anti-reflection effects, light incident on the first surface can also be utilized, increasing the light absorption effect of the back-contact cell on the first surface. This allows the back-contact cell to absorb light energy from both sides, further utilizing light energy and improving the power generation efficiency of the back-contact cell.

[0091] As some possible implementations, as shown in Figures 1 to 3, the surface of the first doped region 101 and / or the surface of the second doped region 102 and / or the surface of the stacked region 104 are polished surfaces. In this case, the surfaces of the first doped region 101, the second doped region 102 and the stacked region 104 can all be polished surfaces, so that the light incident from the second surface and passing through the back contact cell is re-reflected, so that the light has the opportunity to be reused by the back contact cell, thereby improving the photoelectric conversion efficiency of the back contact cell. In addition, the polished surface has better flatness, and the subsequent formation of other layers on the polished surface will have a better effect, which is conducive to reducing the generation of interface defects, thereby reducing the recombination of carriers caused by defects, and is conducive to improving the passivation performance of the back contact cell, thereby improving the photoelectric conversion efficiency of the back contact cell.

[0092] As some possible implementations, as shown in FIG3 , the back-contact cell further includes a first interface passivation layer 14, a second interface passivation layer 151, and a third interface passivation layer 152. The first interface passivation layer 14 is located between the substrate 10 and the first doped layer 11. The second interface passivation layer 151 is located between the second doped layer 121 and the first protective layer 16. The third interface passivation layer 152 is located between the substrate 10 and the third doped layer 122. The first interface passivation layer 14, the second interface passivation layer 151, and the third interface passivation layer 152 respectively passivate the substrate 10, the first protective layer 16, and the first doped layer 11, thereby reducing carrier recombination at the interface and ensuring carrier transmission efficiency.

[0093] In some examples, the first interface passivation layer 14, the second interface passivation layer 151, and the third interface passivation layer 152 may be one or more of oxides, nitrides, carbides, and hydrogenated amorphous silicon. Oxides include one or more of silicon oxide, silicon oxynitride, aluminum oxide, titanium oxide, hafnium dioxide (HfO2), gallium oxide (Ga2O3), tantalum pentoxide (Ta2O5), and niobium pentoxide (Nb2O5); nitrides include one or more of silicon nitride, silicon carbonitride, aluminum nitride, titanium nitride (TiN), and titanium carbonitride (TiCN); and carbides include silicon carbide (SiC).

[0094] In some examples, when the first doped layer 11, the second doped layer 121, and the third doped layer 122 are semiconductor doped layers, the first interface passivation layer 14, the second interface passivation layer 151, and the third interface passivation layer 152 may be tunneling oxide layers. The tunneling oxide layer allows majority carriers to tunnel into the semiconductor doped layer while blocking minority carriers from passing through. As a result, majority carriers are transported laterally within the semiconductor doped layer and collected by the electrode, reducing carrier recombination and improving the open circuit voltage and short circuit current of the back contact battery. At this time, the tunneling oxide layer and the semiconductor doped layer constitute a tunneling oxide layer passivation contact structure, which can achieve excellent interface passivation and selective collection of carriers, thereby improving the photoelectric conversion efficiency of the back contact battery. The first interface passivation layer 14, the second interface passivation layer 151, and the third interface passivation layer 152 may all be silicon oxide interface passivation layers. Compared with the amorphous silicon interface passivation layer that crystallizes and transforms into polycrystalline silicon at high temperatures, the silicon oxide interface passivation layer is more resistant to high temperatures.

[0095] As some possible implementations, as shown in Figures 1 to 3, the back-contact cell further includes a first surface passivation layer 13. The first surface passivation layer 13 covers the first doped layer 11, the second doped layer 121, the third doped layer 122, and the third region 103. The first surface passivation layer 13 has a first opening 130 at the interface between the first surface passivation layer 13 and the first doped layer 11. The first electrode 20 is in electrical contact with the first doped layer 11 through the first opening 130. The first surface passivation layer 13 has a second opening 131 at the interface between the first surface passivation layer 13 and the third doped layer 122. The second electrode 21 is in electrical contact with the third doped layer 122 through the second opening 131.

[0096] Based on this, a first surface passivation layer 13 is formed on the outside of the first doped layer 11, the second doped layer 121, the third doped layer 122, and the third region 103. The first surface passivation layer 13 can passivate the surface of the back-contact battery, passivate the dangling bonds in the first doped layer 11, the second doped layer 121, the third doped layer 122, and the third region 103, reduce the carrier recombination velocity on the first surface, and improve the photoelectric conversion efficiency. The first electrode 20 and the second electrode 21 are electrically contacted with the first doped layer 11 and the third doped layer 122 through the first opening 130 and the second opening 131, respectively, forming a local ohmic contact between the metal and the semiconductor, reducing the contact area between the metal electrode and the first doped layer 11 and the third doped layer 122, reducing the contact resistance, further reducing the carrier recombination rate at the electrode surface, and improving the open circuit voltage. At the same time, the first surface passivation layer 13 located in the third region 103 also serves to isolate the second doped layer 121 and the third doped layer 122.

[0097] In some examples, the material of the first surface passivation layer 13 may be one or more of silicon nitride, silicon oxide, silicon oxynitride, aluminum oxide, silicon carbide, and amorphous silicon.

[0098] As some possible implementations, as shown in Figures 1 to 3, the second surface has a suede structure. A second surface passivation layer 18 is also provided on the second surface. The suede structure of the second surface has a good light trapping effect, which can reduce the reflection of light incident on the second surface and improve the utilization rate of light. The second surface passivation layer 18 provides the second surface with the function of passivating the interface of the substrate 10, reducing the recombination of carriers at the interface, improving the carrier transmission efficiency, and thereby improving the photoelectric conversion efficiency of the back contact cell.

[0099] In some examples, the material of the second surface passivation layer 18 may be one or more of silicon nitride, silicon oxide, silicon oxynitride, aluminum oxide, silicon carbide, and amorphous silicon.

[0100] As some possible implementations, the second surface of the back-contact cell further includes an anti-reflection layer. The anti-reflection layer can be formed on the second-surface passivation layer 18. The anti-reflection layer can reduce reflection of light incident on the second surface, improve light refraction, and increase the utilization rate of light incident on the second surface, thereby improving the photoelectric conversion efficiency of the back-contact cell.

[0101] In some examples, the first surface passivation layer 13 and the second surface passivation layer 18 also have an anti-reflection effect. The passivation layer and the anti-reflection layer can also be stacked to achieve an overall anti-reflection effect.

[0102] In some examples, the anti-reflection layer can be one or more materials such as magnesium fluoride (MgF2), silicon dioxide (SiO2), aluminum oxide (Al2O3), zinc sulfide (ZnS), silicon nitride (SiN), titanium dioxide (TiO2), etc.

[0103] Illustratively, the anti-reflection layer may be an aluminum oxide anti-reflection layer, or may be an anti-reflection layer composed of a stack of silicon nitride and silicon oxide.

[0104] As some possible implementations, as shown in Figures 1 to 3, the area of ​​the stacked region 104 accounts for 5% to 95% of the area of ​​the first doped layer 11. Preferably, the area of ​​the stacked region 104 accounts for 20% to 95% of the area of ​​the first doped layer 11. The larger the area of ​​the stacked region 104, the larger the area of ​​the first doped layer 11 covered by the second doped layer 121, that is, the larger the area of ​​the first doped layer 11 protected, which can better protect the first doped layer 11 from corrosion or damage during subsequent processing. More preferably, the area of ​​the stacked region 104 accounts for 40% to 75% of the area of ​​the first doped layer 11. The first protective layer 16 and the second doped layer 121 above the stacked region 104 should avoid contact with the first electrode 20. In addition, if the area of ​​the stacked region 104 is too large, there is a risk of leakage. For example, the width of the first doped region 101 can range from 80μm to 300μm, and the width of the stacked region 104 can range from 60μm to 860μm.

[0105] For example, as shown in FIG. 1 to FIG. 3 , the area of ​​the stacked region 104 may account for 40%, 60% or 75% of the area of ​​the first doped layer 11 .

[0106] In practical applications, the portion arranged according to the stacked region 104 , the first doped region 101 , the stacked region 104 , the third region 103 , the second doped region 102 and the third region 103 may be referred to as a period. The width of a period ranges from 400 μm to 2400 μm.

[0107] As shown in FIG4 to FIG13 , based on the back-contact battery described in any of the above embodiments, the present application also provides a method for manufacturing a back-contact battery, including the following steps:

[0108] Step S100, providing a substrate 10, wherein the substrate 10 has a first surface and a second surface opposite to each other, wherein the first surface has first doped regions 101 and second doped regions 102 arranged alternately, and a stacked region 104 and a third region 103 between the first doped regions 101 and the second doped regions 102, wherein the stacked region 104 is adjacent to the first doped region 101;

[0109] Step S200 , forming a first doping layer 11 on the first surface of the substrate 10 ;

[0110] Step S300 , removing the first doping layer 11 located in the second doping region 102 and the third region 103 ;

[0111] Step S400 , forming a doped film layer 12 on the first doped layer 11 and the first surface;

[0112] Step S500 , removing the doped film layer 12 located on the third region 103 and the first doped region 101 , so that the doped film layer 12 located on the stacked region 104 becomes the second doped layer 121 , and the doped film layer 12 located on the first surface becomes the third doped layer 122 ;

[0113] In step S600 , a first electrode 20 is formed on the first doping layer 11 , and a second electrode 21 is formed on the third doping layer 122 .

[0114] Compared with the prior art, the beneficial effects of the method for manufacturing a back-contact battery provided in the embodiment of the present application are the same as the beneficial effects of the above-mentioned back-contact battery, which will not be described in detail here.

[0115] Among them, in actual application, the substrate 10 needs to be polished and cleaned to remove damage. The thickness range of the first doping layer 11, the second doping layer 121 and the third doping layer 122 is 50nm to 500nm. The process of forming the first doping layer 11 on the substrate 10 and the process of forming the doping film layer 12 on the first doping layer 11 and the first surface can be a plasma chemical vapor deposition (PECVD) process, a hot wire chemical vapor deposition process, a physical vapor deposition (PVD) process, a low pressure chemical vapor deposition (LPCVD) process or a catalytic chemical vapor deposition process. The process of removing the first doping layer 11 located in the second doping region 102 and the third region 103 and the process of removing the doping film layer 12 located on the third region 103 and the first doping region 101 can be a laser etching process, an ion milling etching process, a plasma etching process, a reactive ion etching process, an alkali etching process and an acid etching process.

[0116] In practical applications, as shown in FIG13 , the width of the first electrode 20 and the second electrode 21 ranges from 5 μm to 100 μm. The first electrode 20 and the second electrode 21 may be continuous contact electrodes. In this case, as shown in FIG16 , the first electrode 20 includes a first electrode main electrode 201 and a first electrode sub-gridline 202, and the second electrode 21 includes a second electrode main electrode 211 and a second electrode sub-gridline 212. The first electrode 20 and the second electrode 21 may also be local contact electrodes. As shown in FIG17 , taking the first electrode 20 as an example, the first electrode 20 may include a connecting electrode 203 and a fine gridline 204. The fine gridline 204 is connected to the connecting electrode 203 and conducts current through the connecting electrode 203. The continuous electrode does not contact the first doped layer 121, the fine gridline 204 contacts the first doped layer 121, or a portion of the fine gridline 204 contacts the first doped layer 121, while the remaining portion does not. Exemplarily, as shown in FIG17 , the connecting electrode 203 plays a collecting role, and the fine grid line 204 plays a transmission role and does not contact the first doping layer 121. Only a local contact point 205 on the fine grid line 204 contacts the first doping layer 121. A pad or an electrode output contact can also be provided on the main electrode to enable the output of the battery's electrical energy. The fine grid line 204 can be prepared using different electrode pastes. For example, the fine grid line 204 is composed of conductive paste one and conductive paste two after metallization heat treatment, wherein conductive paste one has the property of penetrating the dielectric film, and conductive paste two does not have the property of penetrating the dielectric film. Conductive paste one is discontinuously distributed, and conductive paste two partially or completely covers conductive paste one and connects the area of ​​conductive paste one.

[0117] In practical applications, the processes for forming the first electrode 20 and the second electrode 21 can be electroplating, transfer (e.g., laser transfer, thermal transfer, etc.), screen printing, physical vapor deposition of metal or metal oxide electrodes, etc. Obviously, various processes can also be used in combination, such as first printing electrodes to form power supply points, then applying power to the power supply points and using electroplating to form the final first electrode 20 and second electrode 21; or using vapor deposition of metal oxides, such as transparent conductive oxides (TCOs), and then forming the first electrode 20 and second electrode 21 by screen printing or transfer.

[0118] In some examples, the first doped layer 11 and the doped film layer 12 are formed by an in-situ doping method or an ex-situ doping method. That is, the first doped layer 11 and the doped film layer 12 can be formed directly, or an intrinsic semiconductor layer and an intrinsic semiconductor film layer can be formed first, and then doped to form the first doped layer 11 and the doped film layer 12.

[0119] As some possible implementations, as shown in FIG. 4 to FIG. 6 , the first doped layer 11 located in the second doped region 102 and the third region 103 is removed. Specifically, a first protective layer 16 is formed on the first doped layer 11 in the first doped region 101 and the stacked region 104. The first doped layer 11 and the first protective layer 16 are removed from the second doped region 102 and the third region 103.

[0120] In practical applications, the first protective layer 16 can be formed using a plasma chemical vapor deposition (PECVD) process, an atmospheric pressure chemical vapor deposition (APCVD) process, or a thermal growth process. The first protective layer 16 can be removed using methods such as acid washing, alkaline washing, and water washing, or by using an ultraviolet laser with a short pulse width. When silicon oxide is used as the first protective layer 16, a thermal growth process can be used to form the first protective layer 16. Specifically, a layer of silicon oxide is formed on the surface of the first doped layer 11 by heating in an oxidizing atmosphere (such as air or oxygen).

[0121] In some examples, when the first protective layer 16 is silicon oxide and the first doped layer 11 is a boron-doped p-type polysilicon layer, the first protective layer 16 and the first doped layer 11 can also be formed in a single process. For example, after forming an intrinsic polysilicon layer, a thermal diffusion process is used to introduce a gas such as BCl3 or BBr3 under heating (oxygen is inevitably introduced during the thermal diffusion process) to dope the intrinsic polysilicon layer, thereby forming a p-type polysilicon layer. At the same time, a layer of silicon oxide is formed on the surface of the p-type polysilicon layer.

[0122] When the substrate 10 is a p-type silicon substrate 10, a phosphorus-doped thermal diffusion process can be used instead. In this case, the in-situ doped p-type polysilicon layer can also be replaced with an n-type polysilicon layer. The POCl3 used for thermal diffusion can also form a phosphorus-doped n-type polysilicon layer and the silicon oxide located thereon.

[0123] Furthermore, when removing the first protective layer 16 of a laminated structure in which the dielectric layer is silicon oxide, the mask layer can be patterned first, and then the first surface of the back contact cell can be cleaned using a fluorine-containing solution, such as hydrofluoric acid (HF) or ammonium fluoride (NH4F), to remove the silicon oxide where the mask material is not provided, facilitating better passivation in subsequent steps. The mask layer can then be removed using an alkaline wash.

[0124] Alternatively, a laser etching process may be used to remove the first doping layer 11 and the first protective layer 16 on the second doping region 102 and the third region 103 at one time, but this may cause greater damage to the substrate 10 .

[0125] As some possible implementations, as shown in Figures 6 to 10, the doped film layer 12 located on the third region 103 and the first doped region 101 is removed, specifically: a second protective layer 17 is formed on the doped film layer 12 located in the stacked region 104 and the second doped region 102. The doped film layer 12 located on the third region 103 and the first doped region 101 is removed. The second protective layer 17 is removed. The material selection, process treatment method and embodiment of the second protective layer 17 are the same as those of the first protective layer 16. The second protective layer 17 is used to protect the second doped layer 121 and the third doped layer 122 so that the second doped layer 121 and the third doped layer 122 will not be corroded or damaged in subsequent cleaning or etching processes. Since the second protective layer 17 may carry metal ions or other contamination, in order to ensure better passivation of the back contact battery in subsequent processes, the second protective layer 17 is removed after it is no longer needed.

[0126] In some examples, the second protective layer 17 includes a mask layer. Preferably, the mask layer is a layer of silicon nitride (SiN) deposited by a PECVD process. x ), silicon oxide (SiO x ) or a silicon carbide (SiC) mask layer. The process for removing the second protective layer 17 can be laser etching. In the process of removing the second protective layer 17, the second protective layer 17 located in the first doping region 101 can be removed first, and then the second protective layer 17 located in the third region 103 can be removed. The second protective layer 17 located in the first doping region 101 and the third region 103 can also be removed simultaneously. Preferably, the second protective layer 17 located in the first doping region 101 and the third region 103 is removed simultaneously.

[0127] As some possible implementations, as shown in Figures 4 to 6, before forming the first doping layer 11 on the first surface of the substrate 10, the step of forming a first interface passivation layer 14 on the first surface of the substrate 10 is further included; in the step of removing the first doping layer 11 located in the second doping region 102 and the third region 103, the step of removing the first interface passivation layer 14 located in the second doping region 102 and the third region 103 is further included. The process for forming the first interface passivation layer 14 can be a plasma chemical vapor deposition (PECVD) process, an atmospheric pressure chemical vapor deposition (APCVD) process, a thermal growth process, etc. The process for removing the first interface passivation layer 14 can be a laser etching process, an ion milling etching process, a plasma etching process, a reactive ion etching process, an alkali etching process, an acid etching process, etc.

[0128] In some examples, the first interface passivation layer 14 may be a tunneling oxide layer, and the thickness of the tunneling oxide layer ranges from 0.5 nm to 5 nm.

[0129] In addition, when the first interface passivation layer 14 is a tunneling oxide layer and the first doping layer 11 is a boron-doped p-type polysilicon layer, the first interface passivation layer 14 and the first doping layer 11 can be formed in one process, that is, the tunneling oxide layer and the boron-doped p-type polysilicon layer are directly grown.

[0130] As some possible implementations, as shown in Figures 6 to 10, after removing the first doping layer 11 located in the second doping region 102 and the third region 103, and before forming the doping film layer 12 on the first doping layer 11 and the first surface, the step of forming an interface passivation film layer 15 on the first protective layer 16 and the first surface is further included; in the step of removing the doping film layer 12 located in the third region 103 and the first doping region 101, the step of removing the interface passivation film layer 15 located in the third region 103 and the first doping region 101 is further included, so that the interface passivation film layer 15 on the first protective layer 16 located in the stacking region 104 is the second interface passivation layer 151, and the interface passivation film layer 15 located on the first surface is the third interface passivation layer 152. The process for forming the interface passivation film layer 15 can be a plasma chemical vapor deposition (PECVD) process, an atmospheric pressure chemical vapor deposition (APCVD) process, a thermal growth process, etc. The process for removing the interface passivation film layer 15 may be a laser etching process, an ion milling etching process, a plasma etching process, a reactive ion etching process, an alkali etching process, an acid etching process, or the like.

[0131] In some examples, the interface passivation film layer 15 may be a tunneling oxide layer with a thickness ranging from 1 nm to 2 nm.

[0132] In addition, when the interface passivation film layer 15 is a tunneling oxide layer and the doped film layer 12 is a phosphorus-doped n-type polysilicon layer, the interface passivation film layer 15 and the doped film layer 12 can be formed in one process, that is, the tunneling oxide layer and the phosphorus-doped n-type polysilicon layer are directly grown.

[0133] As some possible implementations, alkaline etching is used as a method for removing the first doped layer 11 located in the second doped region 102 and the third region 103 and / or removing the doped film layer 12 located in the third region 103 and the first doped region 101. During the alkaline etching process, since the first interface passivation layer 14 and the interface passivation film layer 15 are both relatively thin, they can be cleaned away together with the alkali.

[0134] As some possible implementations, after removing the doped film layer 12 located on the third region 103 , the method further includes the step of texturing the third region 103 .

[0135] Preferably, texturing the third region 103 and removing the doped film layer 12 located in the third region 103 can be completed in the same process. For example, when removing the doped film layer 12 located in the third region 103 by alkaline etching, a textured structure can be formed on the third region 103 at the same time.

[0136] As some possible implementations, as shown in Figures 11 to 13, a first electrode 20 is formed on the first doped layer 11, and a second electrode 21 is formed on the third doped layer 122. Specifically, a first surface passivation layer 13 is formed on the first doped layer 11, the second doped layer 121, the third doped layer 122, and the third region 103. The first electrode 20 is formed on the first surface passivation layer 13 located on the first doped layer 11. The second electrode 21 is formed on the first surface passivation layer 13 located on the third doped layer 122. The first electrode 20 is in electrical contact with the first doped layer 11. The second electrode 21 is in electrical contact with the third doped layer 122.

[0137] In practical applications, the process for forming the first surface passivation layer 13 can be a plasma chemical vapor deposition (PECVD) process, a hot wire chemical vapor deposition process, a physical vapor deposition (PVD) process, a low pressure chemical vapor deposition (LPCVD) process, or a catalytic chemical vapor deposition process. When the back-contact cell has the first surface passivation layer 13 and the first electrode 20 and the second electrode 21 are continuous contact electrodes, the method for forming the first electrode 20 and the second electrode 21 can also be to coat the electrode slurry on the first surface passivation layer 13 and then sinter it so that the electrode slurry passes through the first surface passivation layer 13 and forms electrical contact with the first doping layer 11 and the third doping layer 122, respectively. When a back-contact cell has a first surface passivation layer 13 and the first and second electrodes 20 and 21 are local contact electrodes, the method for forming the first and second electrodes 20 and 21 can also be to first create first openings 130 and 131 in the first surface passivation layer 13, and then form the local contact first and second electrodes 20 and 21 using methods such as printing slurry, laser transfer, electroplating, chemical plating, photoinduced plating, or physical vapor deposition (PVD) such as vacuum evaporation or magnetron sputtering. The pore-forming method can include laser pore-forming or pore-forming using an etching slurry that reacts with the first surface passivation layer 13. Providing electrical contact through pore-forming allows for low metal area recombination in the back-contact cell, ensuring high conversion efficiency. Obviously, a combination of one or more of the above methods can also be used to form the first and second electrodes 20 and 21. For example, a method using a physical vapor deposition (PVD) seed layer in conjunction with printed electrodes, screen printing of electrode slurry in conjunction with electroplating, or a combination of laser transfer and screen printing sintering can be used.

[0138] When the substrate 10 is an n-type silicon substrate 10 and the first doped layer 11 is a p-type polysilicon layer, using the above-described method for forming electrodes by film-forming, a p-type contact region is formed on the first doped region 101 and the stacked region 104. Through the tunneling effect of carriers, the first polarity carriers of the first doped region 101 are collected by the first electrode 20 through the first doped layer 11. An n-type contact region is formed on the second doped region 102, and the second polarity carriers of the second doped region 102 are collected by the second electrode 21 through the third doped layer 122. Subsequently, a conductive paste can be printed on the first surface passivation layer 13 and sintered to form metallized contacts, forming a p-type metal region on the p-type contact region and an n-type metal region on the n-type contact region. Alternatively, a burn-through paste can be directly printed on the first surface passivation layer 13 to form the corresponding p-type metal region and n-type metal region. Ultimately, the first electrode 20 and the second electrode 21 are formed.

[0139] For example, after forming the first electrode 20 and the second electrode 21 , other steps may be performed, such as optical or electrical carrier injection or other heat treatment processes, as well as efficiency binning or slicing steps.

[0140] In some examples, the step of forming the third region 103 can be set before forming the first surface passivation film. The step of forming the third region 103 can also be set after preparing the outer city back contact battery, but this will sacrifice part of the passivation of the third region 103.

[0141] As some possible implementations, before forming the first surface passivation layer 13 on the first doping layer 11, the second doping layer 121, the third doping layer 122 and the third region 103, the step of performing a heat treatment process is also included, wherein the heat treatment process crystallizes at least a portion of the first doping layer 11 and / or the second doping layer 121 and / or the third doping layer 122. The p-type or n-type semiconductor layer can be heat-treated to further distribute the dopant or change the structure of the semiconductor layer, which is more conducive to improving the performance of the battery. For example, when the first doping layer 11, the second doping layer 121 and the third doping layer 122 are amorphous semiconductors or microcrystalline semiconductors, the heat annealing can crystallize at least a portion of the first doping layer 11 and / or the second doping layer 121 and / or the third doping layer 122, thereby improving the electrical conductivity of the first doping layer 11, the second doping layer 121 and the third doping layer 122. In addition, heating annealing can also make the tunnel oxide layer more conducive to selective carrier transmission; heating can also allow doping elements to enter the tunnel oxide layer and the substrate 10, thereby reducing transmission resistance.

[0142] As a possible implementation method, the second surface is further texturized and a second surface passivation layer 18 is formed on the second surface. The process for forming the second surface passivation layer 18 can be a plasma chemical vapor deposition (PECVD) process, a hot wire chemical vapor deposition process, a physical vapor deposition (PVD) process, a low pressure chemical vapor deposition (LPCVD) process, or a catalytic chemical vapor deposition process. Preferably, the patterning process of the third region 103 and the texturizing process of the second surface can be completed in the same process, reducing one or more production processes. This greatly improves commercial production capacity.

[0143] In some examples, the step of texturing the second surface can be performed after the second doping layer 121 and the third doping layer 122 are formed. In the prior art, the step of texturing the second surface is usually performed before the first doping layer 11 is formed on the first surface, so that the textured surface of the second surface is easily damaged during the removal process or cleaning process of the first doping layer 11, the second doping layer 121 or the third doping layer 122. In the embodiment of the present application, the process of texturing the second surface is placed after the formation of the second doping layer 121 and the third doping layer 122, which ensures the integrity of the textured structure and its good light trapping performance. In particular, when the textured structure of the second surface is a nano-velvet structure, various cleaning processes and etching and other graphical processes will almost certainly destroy the nano-velvet textured structure. In recent years, nano-microstructures have been increasingly used in the textured structure of the light-receiving surface, so the advantages of post-texturing have become more and more prominent. The nanotextured texture structure has a better light-trapping effect. And because the light-receiving surface of the back-contact cell has no electrode, the color of the second surface will be more beautiful after applying the nanotextured texture structure to the back-contact cell. Therefore, the nanotextured texture structure is more suitable for back-contact cells.

[0144] Preferably, texturing the second surface, texturing the third region 103, and removing the doped film layer 12 located in the first doped region 101 can be completed in the same process. For example, when removing the doped film layer 12 located in the first doped region 101 using an alkaline etching process using a solution such as potassium hydroxide (KOH), sodium hydroxide (NaOH), or tetramethylammonium hydroxide (TMAH), a textured structure can be formed simultaneously on the third region 103 and the second surface.

[0145] In some examples, the step of forming the second surface passivation layer 18 may be performed simultaneously with the step of forming the first surface passivation layer 13 .

[0146] In some examples, after forming the second surface passivation layer 18 , an anti-reflection layer may be further formed on the second surface passivation layer 18 .

[0147] The present application is described below in conjunction with specific embodiments. The embodiments cited are only used to explain the present application and are not used to limit the scope of the present application.

[0148] Taking the production of the n-type back contact cell shown in FIG1 as an example, the production method is specifically described as follows:

[0149] In the first step, an n-type silicon substrate 10 is provided, and then the n-type silicon substrate 10 is subjected to polishing, cleaning and other damage removal treatments in sequence;

[0150] In the second step, a silicon oxide tunneling oxide layer is deposited on the first surface of the n-type silicon substrate 10 using a PECVD device as a first interface passivation layer 14;

[0151] In the third step, as shown in FIG4 and FIG5, a layer of intrinsic polysilicon layer is deposited on the first interface passivation layer 14 using a PECVD device, and then a thermal diffusion process is used to introduce BCl3 gas into the intrinsic polysilicon layer under heating to dope the intrinsic polysilicon layer, thereby forming a boron-doped p-type polysilicon layer and a silicon oxide layer as a first protective layer 16 on the surface of the p-type polysilicon layer.

[0152] In the fourth step, as shown in FIG6 , the silicon oxide layer on the third region 103 and the second doped region 102 is removed by ultraviolet laser, and then the first interface passivation layer 14 , the p-type polysilicon layer and the first protective layer 16 on the third region 103 and the second doped region 102 are removed by alkaline etching;

[0153] Step 5: Using PECVD equipment, a silicon oxide layer is deposited on the first protective layer 16, the third region 103, and the second doped region 102 as an interface passivation film layer 15;

[0154] Step 6: Deposit a phosphorus-doped n-type polysilicon layer on the interface passivation film layer 15 using a PECVD device to form a structure as shown in FIG. 7 ;

[0155] In the seventh step, as shown in FIG8 , a silicon nitride mask layer is deposited on the n-type polysilicon layer using a PECVD device as a second protective layer 17 , and then the second protective layer 17 in the first region and the third region 103 is removed using a laser.

[0156] In the eighth step, as shown in FIG9 , an alkaline treatment process is used to remove the n-type polysilicon layer and the interface passivation film layer 15 on the first doped region 101 and the third region 103 , so that the interface passivation film layer 15 on the first protective layer 16 in the stacked region 104 becomes the second interface passivation layer 151 , and the interface passivation film layer 15 on the first surface becomes the third interface passivation layer 152 . At the same time, the third region 103 and the second surface are textured.

[0157] In the ninth step, as shown in FIG10 , the second protective layer 17 is removed by laser;

[0158] In the tenth step, as shown in FIG11 , the first protective layer 16 on the first doped region 101 is removed by an alkaline etching process;

[0159] In the eleventh step, as shown in FIG12 , a layer of silicon nitride is deposited on the first doped region 101 , the stacked region 104 , the third region 103 , and the second doped region 102 using a PECVD device as a first surface passivation layer 13 , and a layer of silicon nitride is deposited on the textured structure on the second surface as a second surface passivation layer 18 ;

[0160] In the twelfth step, as shown in FIG13 , a first opening 130 is opened on the first surface passivation layer 13 at the first doping region 101 by using a laser, and then a first electrode 20 is formed by printing a conductive paste. The first electrode 20 is electrically contacted with the first doping layer 11 through the first opening 130; a second opening 131 is opened on the first surface passivation layer 13 at the second doping region 102 by using a laser, and then a second electrode 21 is formed by printing a conductive paste. The second electrode 21 is electrically contacted with the third doping layer 122 through the second opening 131 to form a back-contact battery.

[0161] In the description of the above embodiments, specific features, structures, materials or characteristics may be combined in an appropriate manner in any one or more embodiments or examples.

[0162] The above description is merely a specific embodiment of the present application, but the scope of protection of the present application is not limited thereto. Any changes or substitutions that can be easily conceived by a person skilled in the art within the technical scope disclosed in this application should be included in the scope of protection of this application. Therefore, the scope of protection of this application should be based on the scope of protection of the claims.

Claims

1. A back contact battery, characterized in that: include: a substrate having a first surface and a second surface opposite to each other, the first surface having first doped regions and second doped regions arranged alternately, and a stacked region and a third region between the first doped regions and the second doped regions, the stacked region being close to the first doped regions; a first doped layer formed on the first doped region and the stacked region; a second doped layer formed on the first doped layer, the second doped layer being located only above the stacked region, and the first doped layer and the second doped layer having opposite conductivity types; a third doped layer formed on the second doped region, the third doped layer having a conductivity type opposite to that of the first doped layer; and a first electrode and a second electrode, wherein the first electrode is in electrical contact with the first doping layer, and the second electrode is in electrical contact with the third doping layer.

2. The back contact battery according to claim 1, characterized in that The invention also includes a first protection layer located above the stacked region and between the first doping layer and the second doping layer.

3. The back contact battery according to claim 2, characterized in that The first protection layer includes at least one of a dielectric layer and a mask layer.

4. The back contact battery according to claim 3, characterized in that The first protective layer includes one of a borosilicate glass layer and a phosphosilicate glass layer.

5. The back contact battery according to claim 1, characterized in that The surface of the third region has a suede structure.

6. The back contact battery according to claim 1, characterized in that The surface of the first doping region and / or the surface of the second doping region and / or the surface of the stacked region are polished surfaces.

7. The back contact battery according to claim 2, characterized in that It also includes a first interface passivation layer, a second interface passivation layer and a third interface passivation layer, the first interface passivation layer is located between the substrate and the first doping layer, the second interface passivation layer is located between the second doping layer and the first protective layer, and the third interface passivation layer is located between the substrate and the third doping layer.

8. The back contact battery according to claim 1, characterized in that The substrate is an n-type substrate, the first doping layer is a p-type doping layer, and the second doping layer and the third doping layer are n-type doping layers; or, The substrate is a p-type substrate, the first doping layer is an n-type doping layer, and the second doping layer and the third doping layer are p-type doping layers.

9. The back contact battery according to claim 1, characterized in that Also included is a first surface passivation layer, wherein the first surface passivation layer covers the first doped layer, the second doped layer, the third doped layer and the third region; A first opening is provided at a contact surface between the first surface passivation layer and the first doping layer, and the first electrode is in electrical contact with the first doping layer through the first opening; A second opening is provided at a contact surface between the first surface passivation layer and the third doping layer, and the second electrode is in electrical contact with the third doping layer through the second opening.

10. The back contact battery according to claim 1, characterized in that The area of ​​the stacked layer accounts for 5% to 95% of the area of ​​the first doping layer.

11. The back contact battery according to claim 1, characterized in that The area of ​​the stacked layer accounts for 40% to 75% of the area of ​​the first doping layer.

12. A method for manufacturing a back contact battery according to any one of claims 1 to 11, characterized in that: include: A substrate is provided, wherein the substrate has a first surface and a second surface opposite to each other, wherein the first surface has first doped regions and second doped regions arranged alternately, and a stacked region and a third region between the first doped regions and the second doped regions, wherein the stacked region is close to the first doped region; forming a first doped layer on the first surface of the substrate; removing the first doping layer located in the second doping region and the third region; forming a doped film layer on the first doped layer and the first surface; removing the doped film layer located on the third region and the first doped region, so that the doped film layer located on the stacked region is the second doped layer, and the doped film layer located on the first surface is the third doped layer; A first electrode is formed on the first doping layer, and a second electrode is formed on the third doping layer.

13. The method for manufacturing a back contact battery according to claim 12, wherein: The removing of the first doping layer located in the second doping region and the third region is specifically: forming a first protective layer on the first doped region and the first doped layer in the stacked region; removing the first doping layer and the first protective layer on the second doping region and the third region; and / or, The removing of the doped film layer located on the third region and the first doped region is specifically as follows: forming a second protective layer on the doped film layer located in the stacked region and the second doped region; removing the doped film layer located on the third region and the first doped region; Remove the second protective layer.

14. The method for manufacturing a back contact battery according to claim 13, wherein: Before forming the first doping layer on the first surface of the substrate, the method further includes the steps of: forming a first interface passivation layer on the first surface of the substrate; The step of removing the first doping layer located in the second doping region and the third region further includes the steps of: removing the first interface passivation layer located in the second doping region and the third region; and / or, After removing the first doping layer located in the second doping region and the third region and before forming the doping film layer on the first doping layer and the first surface, the method further includes the steps of: forming an interface passivation film layer on the first protective layer and the first surface; The step of removing the doped film layer located in the third region and the first doped region also includes the step of removing the interface passivation film layer located in the third region and the first doped region, so that the interface passivation film layer located on the first protective layer in the stacked region is the second interface passivation layer, and the interface passivation film layer located on the first surface is the third interface passivation layer.

15. The method for manufacturing a back contact battery according to claim 12, wherein: The first doping layer and the doping film layer are formed by an in-situ doping method or a non-in-situ doping method.

16. The method for manufacturing a back contact battery according to claim 12, wherein: After removing the doped film layer on the third region, the method further includes the step of performing texturing treatment on the third region.

17. The method for manufacturing a back contact battery according to claim 12, wherein: The first electrode is formed on the first doped layer, and the second electrode is formed on the third doped layer, specifically: forming a first surface passivation layer on the first doping layer, the second doping layer, the third doping layer and the third region; A first electrode is formed on the first surface passivation layer of the first doping layer, and a second electrode is formed on the first surface passivation layer of the third doping layer. The first electrode is in electrical contact with the first doping layer, and the second electrode is in electrical contact with the third doping layer.

18. The method for manufacturing a back contact battery according to claim 17, wherein: Before forming the first surface passivation layer on the first doping layer, the second doping layer, the third doping layer and the third region, the method further includes performing a heat treatment process to crystallize at least a portion of the first doping layer and / or the second doping layer and / or the third doping layer.

19. The method for manufacturing a back contact battery according to claim 12, wherein: The method for removing the first doping layer located in the second doping region and the third region and / or the method for removing the doping film layer located in the third region and the first doping region is alkaline etching.