Method for generating steelmaking slag free lime content estimation model, method for estimating free lime content of steelmaking slag, steelmaking slag shipment management method, and method for manufacturing steelmaking slag for roads

The method uses LIBS to estimate free lime content in steelmaking slag through emission spectrum analysis, addressing the complexity and accuracy issues of existing methods, enabling efficient aging treatment and improved stability and management of steelmaking slag for road applications.

WO2024202481A1PCT designated stage expired Publication Date: 2024-10-03JFE STEEL CORP
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/002416
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-01-26
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Current methods for estimating the free lime content in steelmaking slag are either too complex, time-consuming, or lack accuracy, making it difficult to predict the expandability and determine appropriate aging treatment times for steelmaking slag used as road base materials, which can lead to irregularities and safety issues when exposed to moisture.

Method used

A method utilizing laser-induced breakdown spectroscopy (LIBS) to generate a model for estimating free lime content by analyzing the emission spectrum of steelmaking slag, incorporating peaks from Ca, Fe, Si, Al, and P emission lines, and applying partial least squares regression for high accuracy and efficiency.

Benefits of technology

Enables quick and accurate estimation of free lime content in steelmaking slag, allowing for appropriate aging treatment and improved stability of road steel slag, reducing manufacturing costs and enhancing shipping management efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024002416_03102024_PF_FP_ABST
    Figure JP2024002416_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided are a method for generating a steelmaking slag free lime content estimation model capable of easily and rapidly estimating the free lime content of steelmaking slag with high accuracy, a method for estimating the free lime content of steelmaking slag, a steelmaking slag shipment management method, and a method for manufacturing steelmaking slag for roads. The method for estimating the free lime content of steelmaking slag includes: a light-emission spectrum acquisition step for shining a laser onto the steelmaking slag to plasmatize a portion of the surface of the steelmaking slag, and acquiring light-emission spectra from the resulting plasma; and a free lime content estimation step for inputting into a free lime content estimation model the intensities of light-emission spectra including a peak based on a Ca emission line, a peak based on an Fe emission line, and a peak based on an Si emission line, among the light-emission spectra acqured in the light-emission spectrum acquisition step, and outputting the free lime content of the steelmaking slag onto which the laser has been shone.
Need to check novelty before this filing date? Find Prior Art

Description

Method for generating a model for estimating the free lime content of steelmaking slag, method for estimating the free lime content of steelmaking slag, method for managing the shipping of steelmaking slag, and method for manufacturing steel slag for road use

[0001] The present invention relates to a method for generating a model for estimating the free lime content of steelmaking slag, a method for estimating the free lime content of steelmaking slag, a method for managing the shipment of steelmaking slag, and a method for producing steelmaking slag for road use.

[0002] Among the steel slags produced during the steelmaking process, steelmaking slag, particularly those produced during the refining process, specifically converter slag and electric furnace slag, is crystalline and harder than other slags. Therefore, by cooling the steelmaking slag and then crushing it to a predetermined particle size, the steelmaking slag can be used as a roadbed material. However, some of the quicklime used during refining may remain in the steelmaking slag. This quicklime remaining in the steelmaking slag is called free lime. This quicklime may also be referred to as free calcium oxide, free lime, or f-CaO. When this free lime comes into contact with water, such as rainwater or seawater, it undergoes a hydration reaction and expands in volume. Therefore, when steelmaking slag containing free lime is used as a roadbed material, the volume expansion caused by the hydration reaction of the free lime in the steelmaking slag may result in ridge-like irregularities in the roadbed. There is also the possibility of pop-outs occurring, where the roadbed rises in a mountain-like shape in localized areas and breaks through the asphalt, impeding the flow of vehicles and pedestrians.

[0003] JIS A 5015:2018 "Steel slag for roads" specifies the steel slag used in road bases and hot asphalt mixtures (hereinafter referred to as "steel slag for roads"). Specifically, it specifies the physical and chemical properties and particle size of steel slag for roads depending on the application of the steel slag. For example, when steel slag is used for roads, it specifies that the expansion rate of the steel slag when immersed in water must be 1.0% or less.

[0004] Therefore, in order to stabilize the expansive properties of steelmaking slag, after crushing the slag, it is subjected to an aging treatment in which it is reacted with air and water.

[0005] Here, we will explain the steelmaking slag produced in a converter and its aging process. In a converter, blowing is performed in a batch process for each charge. Therefore, even when the converter is operated under approximately the same conditions, the properties of the steelmaking slag, such as basicity, viscosity, and chemical composition, which are indicators of reactivity, are prone to variation. In addition, equipment errors may occur. Therefore, the free lime content of the steelmaking slag produced for each charge inevitably varies.

[0006] Currently, steelmaking slag is stored in a slag yard as a mixture of multiple charges and aged. Aging processes can be broadly divided into air aging and steam aging. In air aging, steelmaking slag is stored in a slag yard for a predetermined storage period to allow the moisture in the air to react with the free lime. In steam aging, steam is supplied to the steelmaking slag stored in the slag yard for a predetermined period to allow the steam (moisture) to react with the free lime. The expansion of steelmaking slag is correlated with its free lime content. Therefore, regardless of the aging process, it is appropriate to quantify the free lime content of the steelmaking slag and perform the aging process for a period corresponding to the free lime content. Specifically, when determining the storage period in a slag yard, i.e., the aging treatment time, a portion of the steelmaking slag stored in the slag yard is sampled to evaluate its expansion and free lime content, and the aging treatment time is determined based on these results. However, as mentioned above, the steelmaking slag stored in the slag yard is a mixture of steelmaking slag from multiple charges. Therefore, the evaluation of the expansiveness and free lime content described above merely evaluated the expansiveness and free lime content of one of the steelmaking slags among multiple charges of steelmaking slag.

[0007] Therefore, in consideration of the safety when using steelmaking slag as a roadbed material, it is preferable to perform an aging treatment for a longer period of time than the aging treatment time based on the expansion property and free lime content of the steelmaking slag obtained as described above. However, even if such a long aging treatment is performed, the expansion property of the steelmaking slag after the aging treatment may not satisfy the requirements of JIS A 5015:2018. If the above requirements are not satisfied, the aging treatment will have to be performed again.

[0008] If the free lime content of steelmaking slag can be easily and quickly evaluated, it becomes possible to predict the expansiveness of the steelmaking slag produced for each charge. It also becomes possible to perform an aging treatment for each charge for an appropriate time. Furthermore, even in the case of a mixture of steelmaking slag from multiple charges, the total amount, average value, and maximum value of the free lime content of the mixture can be determined using the free lime content of each charge. Therefore, it becomes possible to perform an aging treatment for an appropriate time depending on the total amount, average value, and maximum value.

[0009] Several methods have been disclosed for quantifying the free lime content of steelmaking slag. Non-Patent Document 1 discloses the ethylene glycol extraction method. In this method, steelmaking slag pulverized to 0.074 mm or less is stirred for one hour in ethylene glycol heated to 80°C to dissolve the calcium oxide (CaO) contained in the steelmaking slag. The calcium (Ca) in the ethylene glycol is then quantified to determine the free lime content of the steelmaking slag. The ethylene glycol extraction method is essentially used as the standard method in the steel industry.

[0010] Patent Document 1 discloses a method for quantifying the free lime content of steelmaking slag from the ratio of integrated intensities of nuclear magnetic resonance spectra obtained from a mixture of steelmaking slag and a reagent using solid-state NMR.

[0011] Patent Document 2 describes CaO—SiO 2 -MgO-Al 2 O 3This publication discloses a method for estimating the free lime content of steelmaking slag from the quaternary phase diagram and reducing the hydration expansion of the steelmaking slag by controlling the composition of the steelmaking slag.

[0012] Patent Document 3 discloses a method for analyzing the composition of slag, in which the amount of Ca contained in the slag is converted into the amount of CaO, assuming that all of the Ca contained in the slag is present as CaO.

[0013] As a related technique, Non-Patent Document 2 discloses a method for determining an alternative index (L value) correlated with the free lime content by an estimation formula based on the composition values ​​and stoichiometric ratios of specific mineral phases containing Ca in the slag.

[0014] JP 2012-42464 A JP 2001-64714 ​​A JP 2016-48235 A

[0015] Edited by the Committee for Standardization of Characterization Technology for Free CaO in Steel Slag, Analysis Technology Division, Production Technology Department, Iron and Steel Institute of Japan, "Standardization of Characterization Technology for Free CaO in Steel Slag - Final Report of the Study Group on Standardization of Characterization Technology for Free CaO in Steel Slag -," March 28, 2013, pp. 88-95. Wada Kaname and five others, "Hardness Stabilization Treatment of Molten Converter Slag," Steelmaking Research, No. 3011, 1980, pp. 59-70. Okazaki Kodai and four others, "Study on the Application of Laser-Induced Breakdown Spectroscopy (LIBS) to Material Hardness Evaluation Methods," Atomic Energy Society of Japan, 2019 Spring Annual Meeting, March 2019. Murayama Seiichi and one other, "Plasma Emission Methods for Solid Sample Analysis: Japan Spectroscopic Society Measurement Method Series 2," Society Publishing Center, October 1982.

[0016] The ethylene glycol extraction method described in Non-Patent Document 1 involves the cumbersome nature of wet analysis and lacks speed. In addition, skilled workers are required to obtain highly accurate quantitative values. Furthermore, the free lime (f-CaO) and calcium hydroxide (Ca(OH)) contained in steelmaking slag are 2 ) is extracted at the same time, so Ca(OH) 2 It is necessary to measure the quantitative value of by thermogravimetric analysis and calculate the free lime content, which is a heavy workload.

[0017] The method disclosed in Patent Document 1 requires complicated sample preparation, requires special analytical equipment, and takes several days to perform the measurement, making it slow to perform.

[0018] The method disclosed in Patent Document 2 is a method for estimating the free lime content by assuming a thermodynamically ideal equilibrium state, and has the problem of low accuracy in the case of a complex multi-component system such as steelmaking slag.

[0019] As described above, the slag composition analysis method described in Patent Document 3 is a method for estimating the free lime content on the assumption that all of the Ca contained in the slag is present as CaO. Therefore, the slag composition analysis method described in Patent Document 3 may not be able to determine the free lime content with high accuracy.

[0020] The present invention has been made to solve the above-mentioned problems, and aims to provide a method for generating a model for estimating the free lime content of steelmaking slag, a method for estimating the free lime content of steelmaking slag, a method for managing the shipment of steelmaking slag, and a method for manufacturing steel slag for road use, which are capable of estimating the free lime content of steelmaking slag simply, quickly, and with high accuracy.

[0021] The present inventors focused on the emission spectrum obtained by subjecting steelmaking slag to laser emission spectroscopy and completed the present invention. To achieve the above-mentioned object, the present invention provides: [1] a method for estimating the free-lime content of steelmaking slag, comprising: an emission spectrum acquisition step of irradiating the steelmaking slag with a laser to convert a portion of the steelmaking slag surface into plasma and acquiring an emission spectrum from the plasma; and a free-lime content estimation step of inputting the intensities of emission spectra acquired in the emission spectrum acquisition step, which include peaks based on Ca emission lines, Fe emission lines, and Si emission lines, into a free-lime content estimation model to output the free-lime content of the laser-irradiated steelmaking slag. [2] The method for estimating the free-lime content of steelmaking slag according to [1], wherein in the estimation step, the intensities of emission spectra further including peaks based on Al emission lines and P emission lines are input into the free-lime content estimation model. [3] The method for estimating the free lime content of steelmaking slag according to [1], wherein the free lime content estimation model is a model constructed by partial least squares regression, using the intensity of an emission spectrum obtained in the emission spectrum acquisition step, which includes a peak based on a Ca emission line, a peak based on an Fe emission line, and a peak based on a Si emission line, as an explanatory variable, and the free lime content as a target variable. [4] The method for estimating the free lime content of steelmaking slag according to [3], wherein the free lime content estimation model is a model constructed by partial least squares regression, using the intensity of an emission spectrum further including a peak based on an Al emission line and a peak based on a P emission line as an explanatory variable. [5] The method for estimating the free lime content of steelmaking slag according to [1], wherein the free lime content estimation model is a trained machine learning model, using the intensity of an emission spectrum obtained in the emission spectrum acquisition step, which includes a peak based on a Ca emission line, a peak based on an Fe emission line, and a peak based on a Si emission line, as input data, and the free lime content as output data.[6] The method for estimating the free-lime content of steelmaking slag according to [5], wherein the free-lime content estimation model uses as input data the intensity of an emission spectrum further including a peak based on an emission line of Al and a peak based on an emission line of P. [7] The method for estimating the free-lime content of steelmaking slag according to [1], wherein the wavelength of the emission spectrum acquired in the emission spectrum acquisition step is 270 nm or more and 410 nm or less. [8] A method for producing steelmaking slag for road use, comprising estimating the free-lime content of steelmaking slag by the method for estimating the free-lime content of steelmaking slag according to [1] above, and setting aging treatment conditions for the steelmaking slag based on the estimated free-lime content of the steelmaking slag. [9] A method for managing steelmaking slag shipment, comprising estimating the free-lime content of steelmaking slag by the method for estimating the free-lime content of steelmaking slag according to [1] above, and selecting a shipping destination for the steelmaking slag based on the estimated free-lime content of the steelmaking slag.

[10] A method for generating a free-lime content estimation model for steelmaking slag used to estimate the amount of free-lime contained in steelmaking slag, the method comprising: a first acquisition step of irradiating the steelmaking slag with a laser to convert a portion of the surface of the steelmaking slag into plasma and acquiring an emission spectrum from the plasma; a second acquisition step of acquiring an actual free-lime content of the steelmaking slag from which the emission spectrum was acquired in the first acquisition step; and a model generation step of acquiring a plurality of data sets, each set consisting of the emission spectrum acquired in the first acquisition step and the actual free-lime content acquired in the second acquisition step, and generating a free-lime content estimation model based on these data sets, using as input the intensities of the emission spectra acquired in the first acquisition step, which include a peak based on a Ca emission line, a peak based on an Fe emission line, and a peak based on a Si emission line, and outputting the actual free-lime content acquired in the second acquisition step.

[11] The method for generating a model for estimating the free lime content of steelmaking slag according to

[10] , wherein the model generation step inputs the intensity of an emission spectrum that further includes a peak based on an emission line of Al and a peak based on an emission line of P.

[0022] The present invention provides a method for generating a free lime content estimation model for steelmaking slag, which can easily, quickly, and accurately estimate the free lime content of steelmaking slag. Furthermore, the present invention also provides a method for easily, quickly, and accurately estimating the free lime content of steelmaking slag using the free lime content estimation model. As a result, the free lime content of steelmaking slag for each charge can be easily, quickly, and accurately estimated, and an appropriate aging treatment time can be easily and quickly set based on the free lime content of the steelmaking slag for each charge. Furthermore, even for a mixture of steelmaking slag from multiple charges, an appropriate aging treatment time can be set based on the maximum free lime content. As a result, the expansion properties of steelmaking slag for roads can be stabilized, and efficient aging treatment can be performed, thereby reducing the production costs of steelmaking slag used as roadbed material. Furthermore, the estimated free lime content can be used to select an appropriate shipping destination for steelmaking slag, thereby improving the efficiency of shipping management of steelmaking slag within a plant.

[0023] Fig. 1 is a diagram showing an example of a regression coefficient. Fig. 2 is a diagram showing the relationship between the free lime content estimated by substituting the emission spectra of the steelmaking slag samples shown in Table 1 into the model formula and the actually measured free lime content. Fig. 3 is a diagram showing the emission spectra of Ca, Fe, Si, Al, and P present in the wavelength range of 270 to 410 nm, which were used as explanatory variables to generate the model formula in Example 4 of the invention, and the intensity of the emission spectra.

[0024] The present inventors have investigated a method for easily, quickly, and accurately estimating the free lime content of steelmaking slag. In this investigation, they focused on laser-induced breakdown spectroscopy (LIBS), an elemental analysis method that allows direct analysis in air without sample pretreatment and enables instantaneous simultaneous analysis of multiple elements with simple operations. In LIBS, a high-energy pulsed laser is irradiated onto the steelmaking slag to be analyzed, converting a portion of the slag into plasma. Furthermore, LIBS captures and disperses the excitation light, i.e., plasma emission, obtained from the plasmatized steelmaking slag, allowing quantitative analysis to be performed based on the wavelength and intensity of the emission lines corresponding to each element.

[0025] Each of the elements constituting steelmaking slag exists mainly in the form of an oxide, but each element constituting steelmaking slag exists not only in the form of an oxide of the element alone but also in the form of a composite oxide consisting of multiple elements. For example, calcium (Ca) exists in the form of calcium silicate (e.g., CaSiO 3 ), calcium aluminate (e.g., CaAl 2 O 4 ), and calcium ferrite (e.g., CaFeO 2 ) etc. Therefore, it is difficult to calculate the amount of each element's oxide and composite oxide from the content of each element in the steelmaking slag obtained by LIBS.

[0026] On the other hand, Non-Patent Document 3 suggests that the emission spectrum obtained by LIBS may change depending on the bonding state of the compound. Therefore, the inventors focused on the emission spectrum obtained by LIBS and investigated estimating the free lime content from the relationship between the emission spectrum obtained by LIBS and the free lime content.

[0027] As mentioned above, calcium compounds contained in steelmaking slag include calcium silicate (e.g., CaSiO 3 ), calcium aluminate (e.g., CaAl 2 O 4 ), calcium ferrite (e.g., CaFeO 2 ), and tricalcium phosphate (e.g., Ca3 (P.O. 4 ) 2 ) is known. Therefore, the inventors focused on the emission spectrum of Ca-based compounds obtained using LIBS. Specifically, they created a free-lime content estimation model using the emission spectrum of the Ca-based compound as an explanatory variable and the actual free-lime content as a target variable. The emission spectrum used as an explanatory variable is an emission spectrum that contains at least one peak based on the emission line of Ca, one peak based on the emission line of Fe, and one peak based on the emission line of Si, among peaks based on the emission lines of Ca, Fe, Si, Al, and P, which are elements that constitute the Ca-based compound. They discovered that by doing so, the free-lime content can be estimated.

[0028] The present invention has been made based on the above findings. Preferred embodiments of the present invention will be specifically described below.

[0029] (Steelmaking slag) The steelmaking slag used in this embodiment may be converter slag or electric furnace slag. The steelmaking slag may be in a molten state or a solid state.

[0030] (First Acquisition Step) Using a conventionally known laser emission spectrometer, a pulsed laser is irradiated onto the surface of the steelmaking slag, a portion of the surface of the steelmaking slag is converted into plasma, and an emission spectrum from the plasma is acquired. The pulsed laser may be irradiated onto the surface of the steelmaking slag once or multiple times. The emission spectrum obtained by irradiating the surface of the steelmaking slag with a pulsed laser may be an emission spectrum obtained by a single irradiation of the pulsed laser, or an emission spectrum obtained by integrating multiple emission spectra obtained by multiple irradiations. Furthermore, to improve reliability, multiple emission spectra obtained per irradiation or multiple emission spectra obtained by integrating multiple irradiations may be used. To ensure the reliability of the emission spectrum, it is preferable to use multiple emission spectra obtained by integrating multiple irradiations. Here, the above-mentioned "one irradiation of the pulsed laser" means that the pulsed laser is emitted onto the steelmaking slag once. Furthermore, in the case of a double-pulse laser, in which the pulsed laser is irradiated twice in succession in close time, i.e., within a short period of time, the pulsed laser is irradiated onto the steelmaking slag twice within a short period of time.

[0031] When used for LIBS, the interval between pulse lasers in a double pulse laser is preferably several microseconds to several tens of microseconds, and more preferably, for example, 2 microseconds.

[0032] LIBS can be applied to steelmaking slag in both a molten and solid state. Therefore, in the case of molten steelmaking slag, for example, the molten steelmaking slag received in a slag ladle after converter blowing is directly irradiated with a pulsed laser to obtain an emission spectrum. On the other hand, in the case of solid steelmaking slag, the steelmaking slag is sampled from the slag ladle and cooled. The resulting small pieces of steelmaking slag are irradiated with a pulsed laser to obtain an emission spectrum. Due to component imbalances, the variation (difference) in the emission spectra between sampled steelmaking slag in solid state tends to be greater than that in molten steelmaking slag. Therefore, multi-point analysis is preferable to reduce the variation. Multi-point analysis means sampling a specified charge of steelmaking slag, i.e., a single steelmaking slag, from multiple different locations. The above-mentioned emission spectra are then obtained from a single location for each sampled steelmaking slag, and the average value is calculated. Alternatively, sampling is performed from one location in a given charge of steelmaking slag, i.e., one steelmaking slag, and the above-mentioned emission spectra are acquired from multiple locations in the sampled steelmaking slag to obtain an average value. Alternatively, these two multipoint analyses are combined to acquire multiple emission spectra and obtain an average value.

[0033] (Second Acquisition Step) In this embodiment, the free lime content of the steelmaking slag whose emission spectrum has been acquired in the first acquisition step is actually measured. Note that the free lime content may also be measured using steelmaking slag from the same lot as the steelmaking slag whose emission spectrum has been acquired in the first acquisition step.

[0034] Specifically, the free lime content of the steelmaking slag is measured by a conventionally known ethylene glycol extraction method. In this embodiment, the ethylene glycol extraction method is used as an example of a method for measuring the free lime content of the steelmaking slag, but this is not limiting. Furthermore, regarding the second and first acquisition steps, one of the two acquisition steps may be performed before the other, or the two acquisition steps may be performed approximately simultaneously, i.e., in parallel.

[0035] (Model generation process) Then, the emission spectrum acquired in the first acquisition process is used as an explanatory variable, and the actual measured value of the free lime content acquired in the second acquisition process is used as a target variable to generate a model for estimating the free lime content of steelmaking slag.

[0036] The explanatory variables may include variables that have a certain correlation with each other, and simple multiple regression analysis may result in a decrease in estimation accuracy due to collinearity based on this correlation. Since the constituent elements in steelmaking slag may include elements that have a certain correlation with each other, the possibility of correlations occurring among the explanatory variables in the analysis of steelmaking slag cannot be denied. Therefore, it is preferable to select an analytical method that, in principle, does not cause the problem of collinearity. Partial least squares regression (PLS) is an example of such an analytical method.

[0037] In partial least squares regression, explanatory variables are transformed into mutually uncorrelated principal component axes, and then regression analysis is performed between the explanatory variables and the response variable using only a small number of principal components. Therefore, it is convenient when estimating a response variable from multiple analytical values ​​in which correlations between explanatory variables are recognized, and there is a possibility of obtaining high estimation accuracy. Therefore, in this embodiment, the free lime content of steelmaking slag is estimated using a model (partial least squares regression model) constructed by partial least squares regression as a free lime content estimation model.

[0038] The emission spectrum input as an explanatory variable to the free lime content estimation model as data for generating a partial least squares regression model will now be specifically described. The emission spectrum is an emission spectrum including at least one peak based on a Ca emission line, one peak based on an Fe emission line, and one peak based on a Si emission line from the emission spectrum of the steelmaking slag acquired in the first acquisition step. This is because it is presumed that the peak based on the Ca emission line, the peak based on the Fe emission line, and the peak based on the Si emission line reflect information corresponding to the Ca-based compound content. Preferably, an emission spectrum further including one or more peaks based on an Al emission line and one or more peaks based on a P emission line is used as the explanatory variable. For example, the emission spectrum may be the entire wavelength range measured in the first acquisition step. Alternatively, the emission spectrum may be the partially continuous wavelength range of 400 to 540 nm from the entire wavelength range measured in the first acquisition step. Alternatively, the emission spectrum in the wavelength range of 270 to 410 nm, which is a partially continuous wavelength range among all the wavelength ranges measured in the first acquisition step, may be used.

[0039] The emission spectrum is a collection of various emission lines that occur during complex transition processes between excitation levels when a laser is used as an energy source. In other words, it is data showing the intensity of plasma emission versus the wavelength of plasma emission specific to each element. When multiple elements are present in steelmaking slag, the above-mentioned emission spectrum includes multiple emission lines specific to each excited element. Each element has its own representative or specific wavelength (hereinafter referred to as the central wavelength), which is different from each other. Therefore, in the emission spectrum, the data showing the emission lines of each element are represented by a waveform (called a peak) centered on the central wavelength of each element. Note that the central wavelengths of the above-mentioned elements Ca, Fe, Si, Al, and P may be, for example, wavelengths described in Non-Patent Document 4.

[0040] In this embodiment, it is preferable to acquire, as explanatory variables, intensity data at at least three points, including the central wavelength (i.e., the peak top) of each element in the emission spectrum and one or more points immediately adjacent to the central wavelength on the peak waveform. Alternatively, it is more preferable to acquire, as explanatory variables, intensity data at five or more points, including the peak top of each element and two or more points immediately adjacent to the central wavelength on the peak waveform. The aforementioned closest points can be determined in advance through experiments. Examples of the closest points include two points immediately adjacent to the central wavelength on the peak waveform at half the height of the peak top. Examples of the closest points include the intersection of the baseline and the peak waveform, and the valley point between adjacent peaks.

[0041] Then, a partial least squares regression model corresponding to the free lime content estimation model of this embodiment that defines the relationship between the explanatory variables and the response variable described above is generated.

[0042] As one embodiment of the present invention, a method for generating a free lime content estimation model using 10 types of steelmaking slag samples will be described.

[0043] In this embodiment, the free lime content (hereinafter referred to as the measured f-CaO value) of ten types of steelmaking slag samples was measured using the conventional ethylene glycol extraction method. The measured f-CaO values ​​(mass %, hereinafter simply referred to as %) are summarized in Table 1. Furthermore, LIBS emission spectra were obtained for the ten types of steelmaking slag samples as described above. A model formula (free lime content estimation model) shown in Equation (1) below was generated using the emission spectra as explanatory variables and the measured f-CaO value (%) of each steelmaking slag sample shown in Table 1 as the target variable. The wavelength range of the emission spectrum of each steelmaking slag sample used as the explanatory variable was 270 to 410 nm, and data on the intensity of the emission spectrum was obtained at 464 points (n = 464) within that wavelength range.

[0044]

[0045] Y = k 0 +k 1×X1+k 2 ×X 2 +k 3 ×X 3 +...k n ×X n ... (1) In formula (1), Y is the free lime content (f-CaO), and X 1 ~X n is the data of the intensity of the emission spectrum, which is an explanatory variable. 0 ~k n is a regression coefficient obtained by expanding the latent variables, and an example of the regression coefficient is shown in Figure 1. 0 ~k n The regression coefficients indicated by can be weighted by specifying latent variables. The relationship between the latent variables and the regression equation is as follows:

[0046] Y = b 0 +b 1 ×T 1 +b 2 ×T 2 +...+b r ×T r ...(2) In equation (2), T 1 ~T r is a latent variable, and b 0 ~b r is the regression coefficient for the latent variable. 1 is the first latent variable, and T 2 is the second latent variable, T r is the r-th latent variable. Each can be expressed as follows: T 1 =w 11 ×X 1 +w 12 ×X 2 +...+w 1n ×X n T 2 =w 21 ×X 1 +w 22 ×X 2 +...+w 2n ×X n T r =w r1 ×X 1 +w r2 ×X 2 +...+wrn ×X n w 11 ~w rn is the weighting of each latent variable to the input variables.

[0047] In addition to the above-mentioned 10 types of steelmaking slag samples, the LIBS emission spectrum of a steelmaking slag (referred to as the steelmaking slag to be measured) with an unknown free lime content was obtained in the same manner as described above. The steelmaking slag to be measured is a steelmaking slag that has undergone an aging treatment, and may be, for example, either a converter slag or an electric furnace slag. The steelmaking slag to be measured may also be in a molten or solid state. The above-mentioned process of obtaining the LIBS emission spectrum of the steelmaking slag to be measured corresponds to the emission spectrum obtaining process of this embodiment.

[0048] (Estimation step) The free lime content (mass %; hereinafter simply referred to as %) of the steelmaking slag to be measured is calculated using the free lime content estimation model shown in the above-mentioned formula (1). Specifically, the LIBS emission spectrum of the steelmaking slag to be measured is substituted as an explanatory variable into the free lime content estimation model shown in formula (1). In this way, the free lime content (%) of the steelmaking slag to be measured, which is the objective variable, is calculated.

[0049] Figure 2 shows the relationship between the measured free lime content (%) of the steelmaking slag samples shown in Table 1 (hereinafter referred to as "measured f-CaO value") and the free lime content (%) estimated by substituting the emission spectrum of the steelmaking slag to be measured into the above-mentioned model formula (hereinafter referred to as "estimated f-CaO value"). Here, the steelmaking slag samples shown in Table 1 were assumed to be steelmaking slags to be measured whose free lime content was unknown. The horizontal axis of Figure 2 is the measured f-CaO value (mass %, hereinafter simply referred to as %), and the vertical axis is the estimated f-CaO value (mass %, hereinafter simply referred to as %). The coefficient of determination (R 2 ) was 0.9718, and it was found that there was an extremely high correlation between the measured f-CaO value (%) and the estimated f-CaO value (%). Thus, according to this embodiment, the free lime content can be predicted with high accuracy.

[0050] In this embodiment, the free lime content of steelmaking slag is estimated for each charge, for example, in a converter or electric furnace, using the above-described free lime content estimation model. Then, an appropriate aging treatment time is set for the steelmaking slag for each charge based on the estimated f-CaO value (%), and aging treatment is performed. For a mixture of steelmaking slag from multiple charges, the aging treatment time is set based on the maximum or average of the estimated f-CaO values ​​(%) for each charge, or the total amount of f-CaO.

[0051] Alternatively, the storage location for steelmaking slag for each charge is selected based on the estimated f-CaO value (%). Specifically, steelmaking slag with the same level of estimated f-CaO value (%) is stored in the same location. This allows for efficient aging treatment. The aging treatment time set based on the estimated f-CaO value (%) and the storage location for steelmaking slag selected based on the estimated f-CaO value (%) correspond to the aging treatment conditions for steelmaking slag in the method for producing steelmaking slag for road use of this embodiment.

[0052] As described above, according to this embodiment, the emission spectrum of each steelmaking slag can be quickly obtained using LIBS. Furthermore, the free lime content (%) can be estimated simply, quickly, and with high accuracy based on the emission spectrum and the free lime content estimation model. Therefore, even if the free lime content (%) of each steelmaking slag differs for each charge, the free lime content (%) of each steelmaking slag can be estimated simply, quickly, and with high accuracy. This also makes it possible to set an optimal aging treatment time for each steelmaking slag. Furthermore, it is possible to optimize the storage location according to the free lime content (%) of each steelmaking slag. Therefore, even if the free lime content (%) of each steelmaking slag differs for each charge, the aging treatment can be made more efficient by preventing the aging treatment time for each steelmaking slag from being too long or too short, thereby reducing the cost of the aging treatment for steelmaking slag.

[0053] The aging treatment described above can sufficiently reduce the free lime content in the steelmaking slag. Therefore, steelmaking slag for road construction, i.e., roadbed material, made using the steelmaking slag is less likely to expand when exposed to water, thereby stabilizing the expansiveness and quality of the steelmaking slag for roadbed material. Furthermore, according to this embodiment, the free lime content (%) can be estimated easily, quickly, and with high accuracy. Furthermore, the estimated free lime content (%) can be used to appropriately and quickly manage the shipping of steelmaking slag, thereby improving the efficiency of shipping management within the plant. For example, even if the estimated free lime content (%) of the steelmaking slag falls outside the allowable range, it is possible to quickly select a shipping destination for the steelmaking slag, such as a calcia modifier, where the expansion of the steelmaking slag is not or is unlikely to be a problem. Furthermore, instead of estimating the free lime content (%) of the steelmaking slag before the aging treatment, the free lime content (%) of the steelmaking slag can be estimated after the aging treatment. This makes it possible to easily and quickly determine whether the free lime content in the steelmaking slag has been sufficiently reduced by the aging treatment. Note that the above-mentioned allowable range refers to the free lime content of the steelmaking slag that satisfies the provisions of JIS A 5015:2018 "Iron and steel slag for road use."

[0054] As described above, in this embodiment, a free-lime content estimation model is generated in advance, with the LIBS emission spectrum of the steelmaking slag as the explanatory variable, i.e., input data, and the free-lime content as the target variable, i.e., output data. Then, the LIBS emission spectrum of the steelmaking slag whose free-lime content (%) is to be estimated is substituted into the free-lime content estimation model. This allows the free-lime content (%) of the steelmaking slag to be estimated simply, quickly, and accurately. Furthermore, the expansiveness of the steelmaking slag can be quickly estimated based on the estimated free-lime content (%). Note that the estimation of the free-lime content (%) of the steelmaking slag using the free-lime content estimation model of the steelmaking slag corresponds to the "method for estimating the free-lime content of the steelmaking slag" in this invention. Because the method for estimating the free-lime content of the steelmaking slag of this invention is a simple method as described above, the free-lime content (%) can be estimated within approximately 40 minutes. Therefore, the free-lime content (%) of the steelmaking slag for each charge can be quickly estimated.

[0055] In this embodiment, a partial least squares regression model is used as the free-lime content estimation model, but a trained machine learning model may be used instead. That is, multiple data sets each consisting of a pair of the explanatory variables and the target variable described above are obtained, and machine learning is performed using these as training data to generate a trained machine learning model as the free-lime content estimation model. Then, the LIBS emission spectrum of steelmaking slag whose free-lime content (%) is unknown may be input to the trained machine learning model, and an estimated value of the free-lime content may be output.

[0056] In addition, in this embodiment, the wavelength range of the emission spectrum of each steelmaking slag sample was set to 270 to 410 nm, and data on the intensity of the emission spectrum at 464 points (n = 464) in that wavelength range was used as the explanatory variable. However, instead of this, the emission spectrum used as the explanatory variable is not particularly limited as long as it includes a peak based on the Ca emission line, a peak based on the Fe emission line, and a peak based on the Si emission line. Furthermore, in this embodiment, 10 types of steelmaking slag samples were used to generate the model equation. However, 10 or more types of steelmaking slag samples may be used, and it is more preferable to use 20 or more types of steelmaking slag samples.

[0057] Below, an example will be described in which the free lime content (%) of steelmaking slag was estimated using the model for estimating the free lime content of steelmaking slag according to this embodiment. Note that the present invention is not limited to the following example.

[0058] The steelmaking slag samples shown in Table 1 were irradiated with a 100 mJ, 15 Hz pulsed laser for 1 second, and the resulting emission spectra were used as explanatory variables. The measured f-CaO values ​​(%) for each steelmaking slag sample shown in Table 1 were used as objective variables. A model formula (free lime content estimation model) was then generated based on these explanatory variables, objective variables, and equation (1). The emission spectra used as explanatory variables in generating the model formula were the intensity data of the emission spectra corresponding to the wavelengths selected for each of Invention Examples 1 to 3. OriginPro2017 (registered trademark) was used to perform partial least squares regression to generate the model formula.

[0059] Three types of steelmaking slag (X, Y, Z) were prepared as samples of steelmaking slag for estimating the free lime content (%). Each steelmaking slag (X, Y, Z) was a block of steelmaking slag approximately 3 cm in size, collected from the steelmaking slag discharged after decarburization blowing. As in the case of generating the model equation, the surface of each steelmaking slag (X, Y, Z) was irradiated with a 100 mJ, 15 Hz pulse laser for one second. The emission spectra acquired over that one second were integrated, and these were used as the emission spectra of each steelmaking slag to be used as explanatory variables.

[0060] Next, the emission spectra obtained from each steelmaking slag (X, Y, Z) were substituted as explanatory variables into the above-mentioned free-lime content estimation model, and the free-lime content (%) of each steelmaking slag (X, Y, Z) was estimated. However, the explanatory variables used were data on the intensity of the emission spectra corresponding to the same wavelengths as the explanatory variables used to generate the model formula. For comparison, the free-lime content (%) of each steelmaking slag (X, Y, Z) was measured using the ethylene glycol extraction method. The estimated f-CaO values ​​(%) and the measured f-CaO values ​​(%) were then compared.

[0061] In Example 1, the emission spectra of each steelmaking slag (X, Y, Z) used as explanatory variables were emission spectra in the wavelength range of 270 to 410 nm, which is a wavelength range that includes all of the emission lines of Ca, Fe, Si, Al, and P. Specifically, 464 pieces of data on the intensity of the emission spectra in the wavelength range of 270 to 410 nm were used as explanatory variables. A free-lime content estimation model was generated from the emission spectra of the slags listed in Table 1 above, and the free-lime content (%) was estimated based on the model formula from the emission spectra of each steelmaking slag (X, Y, Z).

[0062] In Example 2, the emission spectra of each steelmaking slag (X, Y, Z) used as explanatory variables were emission spectra in the wavelength range of 400 to 540 nm, which is a wavelength range that includes all of the emission lines of Ca, Fe, Si, Al, and P. Specifically, 464 points of data on the intensity of the emission spectra in the wavelength range of 400 to 540 nm were used as explanatory variables. In Example 2, the free lime content (%) was estimated in the same manner as in Example 1, except for the explanatory variables used to generate the model and estimate the free lime content.

[0063] In Example 3, the emission spectra of each steelmaking slag (X, Y, Z) used as explanatory variables were the peak tops of peaks originating from Ca, Fe, Si, Al, and P present in the wavelength range of 270 to 410 nm, as well as intensity data at two points immediately before and after each peak top. Specifically, for Ca, the data was intensity data for the Ca peak top (393.4 nm) and the points immediately before and after each peak top (393.1 nm, 393.7 nm). For Fe, the data was intensity data for the Fe peak top (374.9 nm) and the points immediately before and after each peak top (374.6 nm, 375.2 nm). For Si, the data was intensity data for the Si peak top (288.1 nm) and the points immediately before and after each peak top (287.8 nm, 288.4 nm). For Al, the data was intensity data for the Al peak top (309.2 nm) and the points immediately before and after each peak top (308.9 nm, 309.5 nm). For P, the data were the intensity data of the emission spectrum at the P peak top (405.9 nm) and before and after it (405.6 nm, 406.2 nm). A total of 15 pieces of data on the intensity of each emission spectrum were used as explanatory variables. In Example 3, the free lime content (%) was estimated in the same manner as in Example 1, except for the explanatory variables used to generate the model and estimate the free lime content (%).

[0064] In Comparative Example 1, the emission spectra of each steelmaking slag (X, Y, Z) were used as explanatory variables, with peaks derived from Ca. Specifically, the Ca peak top (393.4 nm) and 15 pieces of data on the intensity forming the Ca peak were used as explanatory variables. In Comparative Example 1, the free lime content (%) was estimated in the same manner as in Invention Example 1, except for the explanatory variables used to generate the model and estimate the free lime content (%).

[0065] As Comparative Example 2, the free lime content (%) of each steelmaking slag (X, Y, Z) was estimated using the alternative index (L value) described in Non-Patent Document 2. Specifically, the L value (≈ estimated free lime content) was calculated by substituting the previously determined slag component values ​​(wt%) of each steelmaking slag (X, Y, Z) into the formula for calculating "L" described in Non-Patent Document 2.

[0066] The results for Examples 1 to 3 and Comparative Examples 1 and 2 are summarized in Table 2. As shown in Table 2, for each steelmaking slag (X, Y, Z), the measured f-CaO values ​​(%) for Examples 1 to 3 generally agreed well with the estimated f-CaO values ​​(%) for Comparative Examples 1 and 2. That is, the deviation between the measured f-CaO values ​​(%) for Examples 1 to 3 was smaller than the deviation between the measured f-CaO values ​​(%) for Comparative Examples 1 and 2. The standard deviation σd, which indicates accuracy, for Comparative Examples 1 and 2 was 0.92 and 0.62, respectively, for the three types of steelmaking slag (X, Y, Z). In contrast, the standard deviation σd of the error in Example 1 was 0.38, the standard deviation σd of the error in Example 2 was 0.45, and the standard deviation σd of the error in Example 3 was 0.52. These results demonstrate that the present embodiment can accurately predict the free lime content (%).

[0067]

[0068] Therefore, according to this embodiment, by preparing a free lime content estimation model in advance, the free lime content (%) can be easily estimated based on the emission spectrum of steelmaking slag without performing complicated analytical methods such as the ethylene glycol extraction method. Furthermore, by using partial least squares regression, the free lime content (%) can be estimated with high accuracy.

[0069] Furthermore, while it takes 7 hours to determine the free lime content (%) of steelmaking slag using the ethylene glycol extraction method, in this embodiment, the time required to estimate the free lime content (%) of steelmaking slag was approximately 6 minutes. Therefore, the method for estimating the free lime content (%) of steelmaking slag according to the present invention has a large contribution in terms of time when estimating the free lime content (%). The free lime content (%) can be estimated quickly.

[0070] An example (Example 4) of the steelmaking slag shipping management method according to this embodiment will be described below. In Example 4, the free lime content (%) of the steelmaking slag is estimated using the method for estimating the free lime content of steelmaking slag according to this embodiment, and a shipping destination for the steelmaking slag is selected based on the estimated free lime content (%) of the steelmaking slag. Note that the present invention is not limited to the following example.

[0071] In Example 4, the emission spectra obtained by irradiating 20 charges of steelmaking slag in a slag ladle with a 100 mJ, 15 Hz pulsed laser for 1 second and integrating the data were used as explanatory variables. The actual f-CaO values ​​(%) of each steelmaking slag, measured using the ethylene glycol extraction method, were used as the dependent variable. A model equation (free lime content estimation model) was then generated based on these explanatory variables, the dependent variable, and Equation (1). Figure 3 shows the emission spectra and intensities of Ca, Fe, Si, Al, and P present in the wavelength range of 270 to 410 nm, which were used as explanatory variables to generate the model equation in Example 4. A total of 60 intensity data points, including the peak tops of each peak shown in Figure 3 and two points immediately before and after each peak top (not shown in Figure 3), were used as explanatory variables to generate the model equation in Example 4. Five measurements were performed on each steelmaking slag. In addition, "OriginPro2017" (registered trademark) was used to perform partial least squares regression for generating the model formula.

[0072] Next, the emission spectra obtained from the steelmaking slags (Ch. Nos. 1 to 7) for which the free-lime content (%) was to be estimated were substituted as explanatory variables into the above-described free-lime content estimation model. In this way, the free-lime content (%) of each steelmaking slag (Ch. Nos. 1 to 7) was estimated (estimated f-CaO value). However, the explanatory variables used were emission spectra corresponding to the same wavelengths as the explanatory variables used to generate the model formula. The estimated f-CaO value (%) estimated as described above was compared with the actual measured value of the free-lime content (actual f-CaO value) (%). To measure the free-lime content (%), samples were first collected from the steelmaking slags (Ch. Nos. 1 to 7) before they were sprayed in the slag yard. The free lime content (%) in each steelmaking slag sample (Ch. No. 1 to 7) was measured using the ethylene glycol extraction method (measured f-CaO value). The estimated f-CaO value (%) was compared with the measured f-CaO value (%). The partial least squares regression was performed using "OriginPro2017" (registered trademark).

[0073] The steelmaking slag (Ch. Nos. 1 to 7) was received in a slag ladle for transportation within the steelworks after decarburization in a 300-ton converter-type refining furnace. The slag ladle was attached to a cart and towed by a diesel truck along rails laid between the steelworks and the slag yard. The emission spectra of the steelmaking slag (Ch. Nos. 1 to 7) received in the slag ladle were acquired while the slag ladle was stopped until it was connected to the towing diesel truck. Specifically, a 100 mJ, 15 Hz pulsed laser was irradiated onto the surface of the steelmaking slag in the slag ladle that had been discharged after decarburization blowing. The emission spectra acquired over one second were integrated and used to obtain the emission spectra of the steelmaking slag (Ch. Nos. 1 to 7).

[0074] Then, based on the estimated free-lime content (estimated f-CaO value) (%), if the estimated f-CaO value (%) of the steelmaking slag was below a predetermined threshold, it was determined to be low-free-lime slag. The low-free-lime slag was then discharged to slag yard 1, which was maintained along the rail. If the estimated f-CaO value (%) of the steelmaking slag exceeded a predetermined threshold, it was determined to be high-free-lime slag. The high-free-lime slag was then discharged to slag yard 2, which was maintained along the rail. When the estimated f-CaO value (%) of the steelmaking slag was 5.20, a deterioration in the expansion properties of the steelmaking slag for road use, the product, was observed. Therefore, 5.20 was set as the predetermined threshold.

[0075] The results of Example 4 are shown in Table 3. For each of the steelmaking slags (Ch. Nos. 1 to 7) in Example 4, the estimated f-CaO values ​​(%) were in good agreement with the measured f-CaO values ​​(%). The standard deviation σd, which indicates accuracy, was 0.96 for the seven charges of steelmaking slag (Ch. Nos. 1 to 7).

[0076]

[0077] Furthermore, as described above, in Example 4, the estimated f-CaO value (%) could be estimated on-site, simply, quickly, and with high accuracy. Therefore, it became possible to manage steelmaking slag by transporting steelmaking slag with an estimated f-CaO value (%) equal to or less than the threshold to slag yard 1 and steelmaking slag with an estimated f-CaO value (%) exceeding the threshold to slag yard 2.

[0078] From these results, it was found that according to this embodiment, the free lime content (%) of steelmaking slag can be estimated online easily, quickly, and with high accuracy, and that steelmaking slag can be managed according to the free lime content (%).

[0079] Furthermore, by being able to estimate the free lime content (%) of steelmaking slag easily, quickly, and with high accuracy, it is possible to set an appropriate aging treatment time for each charge of steelmaking slag. This makes it possible to avoid or suppress insufficient aging of steelmaking slag, and to provide steel slag for road use efficiently and with stable quality (expansion). Furthermore, since the optimal shipping destination can be selected according to the free lime content (%) of the steelmaking slag, efficient shipping management is also possible.

Claims

1. A method for estimating the free lime content of steelmaking slag, comprising: an emission spectrum acquisition step of irradiating the steelmaking slag with a laser to convert part of the steelmaking slag surface into plasma, and acquiring an emission spectrum from the plasma; and a free lime content estimation step of inputting the intensities of the emission spectrum acquired in the emission spectrum acquisition step, the emission spectrum including a peak based on a Ca emission line, a peak based on an Fe emission line, and a peak based on a Si emission line, into a free lime content estimation model to output the free lime content of the steelmaking slag irradiated with the laser.

2. A method for estimating the free lime content of steelmaking slag as described in claim 1, wherein in the estimation step, the intensity of an emission spectrum further including a peak based on an emission line of Al and a peak based on an emission line of P is input into a free lime content estimation model.

3. The method for estimating the free lime content of steelmaking slag described in claim 1, wherein the free lime content estimation model is a model constructed by partial least squares regression using the intensities of the emission spectra acquired in the emission spectrum acquisition step, the intensities including a peak based on a Ca emission line, a peak based on an Fe emission line, and a peak based on a Si emission line, as explanatory variables, and the free lime content as a response variable.

4. A method for estimating the free lime content of steelmaking slag as described in claim 3, wherein the free lime content estimation model uses as an explanatory variable the intensity of an emission spectrum further including a peak based on an aluminum emission line and a peak based on a phosphorus emission line.

5. The method for estimating the free lime content of steelmaking slag as described in claim 1, wherein the free lime content estimation model is a trained machine learning model that uses as input data the intensities of the emission spectrum acquired in the emission spectrum acquisition step, the intensities including a peak based on a Ca emission line, a peak based on an Fe emission line, and a peak based on a Si emission line, and outputs the free lime content.

6. A method for estimating the free lime content of steelmaking slag as described in claim 5, wherein the free lime content estimation model uses as input data the intensity of an emission spectrum further including a peak based on an aluminum emission line and a peak based on a phosphorus emission line.

7. A method for estimating the free lime content of steelmaking slag as described in claim 1, wherein the wavelength of the emission spectrum acquired in the emission spectrum acquisition process is 270 nm or more and 410 nm or less.

8. A method for manufacturing steel slag for road use, comprising estimating the free lime content of steel slag using the method for estimating the free lime content of steel slag as described in claim 1, and setting aging treatment conditions for the steel slag based on the estimated free lime content of the steel slag.

9. A method for managing the shipping of steelmaking slag, which estimates the free lime content of steelmaking slag using the method for estimating the free lime content of steelmaking slag as described in claim 1, and selects a shipping destination for the steelmaking slag based on the estimated free lime content of the steelmaking slag.

10. A method for generating a free lime content estimation model for steelmaking slag used to estimate the amount of free lime contained in steelmaking slag, comprising: a first acquisition step of irradiating the steelmaking slag with a laser to convert a part of the surface of the steelmaking slag into plasma and acquiring an emission spectrum from the plasma; a second acquisition step of acquiring an actual free lime content of the steelmaking slag whose emission spectrum has been acquired in the first acquisition step; and a model generation step of acquiring a plurality of data sets each consisting of a pair of the emission spectrum acquired in the first acquisition step and the actual free lime content acquired in the second acquisition step, and generating a free lime content estimation model based on these data sets, using as input the intensity of an emission spectrum including a peak based on a Ca emission line, a peak based on an Fe emission line, and a peak based on a Si emission line from the emission spectrum acquired in the first acquisition step, and outputting the actual free lime content acquired in the second acquisition step.

11. A method for generating a model for estimating the free lime content of steelmaking slag as described in claim 10, wherein the model generation process inputs the intensity of an emission spectrum further including a peak based on an Al emission line and a peak based on a P emission line.

Citation Information

Patent Citations

  • Method for quantitative analysis of sulfur and phosphorus in steel and iron by combining random forest algorithm with laser induced breakdown spectroscopy

    CN104697964A

  • Method for recognizing slag variety by combining with laser-induced breakdown spectroscopy based on least squares support vector machine

    CN104697965A

  • Method of improving precision of quantitative analysis of overlapping peak of laser induced breakdown spectrometry

    CN106814061A

  • LIBS multi-component quantitative inversion method based on deep learning convolutional neural network

    CN110705372A

  • Blast furnace molten iron silicon content online detection method and system

    CN113092448A