Method for manufacturing semiconductor substrate, semiconductor substrate, and semiconductor device

The method of ion implanting silicon, carbon, and oxygen into 4H-SiC substrates to form an amorphous layer for bonding and peeling addresses the high cost and reuse challenges in SiC substrate manufacturing, achieving cost-effective and high-quality semiconductor substrates and devices.

WO2024202590A1PCT designated stage expired Publication Date: 2024-10-03SHIN ETSU HANDOTAI CO LTD
View PDF 14 Cites -1 Cited by

Patent Information

Application Number
PCT/JP2024/004569
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-24
Filing Date
2024-02-09
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

The high cost and difficulty in manufacturing high-quality semiconductor substrates using 4H-SiC due to the challenges in bonding and peeling processes, which result in increased substrate costs and limited reuse of peeled substrates, hindering the widespread adoption of SiC in semiconductor devices.

Method used

A method involving ion implantation of silicon, carbon, and oxygen into 4H-SiC substrates to form an amorphous layer, allowing for bonding and peeling of the substrate at a lower cost, with subsequent plasma etching and epitaxial growth to achieve high-quality substrates, enabling the reuse of peeled substrates and reducing manufacturing costs.

Benefits of technology

This approach significantly reduces the cost of producing high-quality semiconductor substrates and devices by facilitating the reuse of peeled substrates, improving substrate quality, and simplifying the peeling process, thereby making SiC substrates more viable for semiconductor applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024004569_03102024_PF_FP_ABST
    Figure JP2024004569_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides a method for manufacturing a semiconductor substrate, the method comprising: an ion implantation step in which ions of at least one of silicon, carbon, and oxygen are implanted into the surface of a 4H-SiC substrate, and an amorphous layer in which silicon and carbon have been amorphized is formed in the 4H-SiC substrate; a joining step in which the 4H-SiC substrate that has been subjected to the ion implantation step and another supporting substrate are joined to each other with a thin film interposed therebetween so as to obtain a joined substrate; a separation step in which the 4H-SiC substrate is separated from the joined substrate at the amorphous layer so as to separate the joined substrate into a bonded substrate in which the surface layer of the 4H-SiC substrate is transferred onto the supporting substrate and a separated substrate that is the 4H-SiC substrate left after the separation of the surface layer; an etching step in which the separation surface of at least one of the bonded substrate and the separated substrate after the separation step is subjected to plasma etching; and an epitaxial step in which at least one of the bonded substrate and the separated substrate is subjected to epitaxial growth. As a result, the present invention provides a method for manufacturing a semiconductor substrate, with which it is possible to manufacture a semiconductor substrate of higher quality at lower cost.
Need to check novelty before this filing date? Find Prior Art

Description

Semiconductor substrate manufacturing method, semiconductor substrate, and semiconductor device

[0001] The present invention relates to a method for manufacturing a semiconductor substrate, a semiconductor substrate, and a semiconductor device.

[0002] SiC has a wide band gap of 2.2 to 3.3 eV, which gives it high dielectric breakdown strength. It also has high thermal conductivity, making it a promising semiconductor material for various semiconductor devices such as power devices and high-frequency devices.

[0003] However, Non-Patent Document 1 reports that in devices using SiC, the manufacturing process of the SiC substrate and the subsequent epitaxial process account for half of the cost, and therefore reducing the cost of the substrate is extremely important.

[0004] As a cost reduction measure, H + A method has been proposed in which ion implantation is performed and the substrate is peeled off. + There have been some prior art reports on the implantation of ions into SiC.

[0005] Patent Document 1 describes a method for producing a substrate for a semiconductor electronic device, in which two SiC single crystal wafers are prepared, an oxide layer is formed on each, hydrogen ions are implanted into one of the substrates, the wafers are then bonded together at room temperature via the oxide layer, and then heat-treated at 500° C. or higher to divide the SiC single crystal wafer in two at the hydrogen ion-implanted location. In this method, an oxide film is present at the bonded portion, and when a vertical device is fabricated, this oxide film functions as an insulating layer, significantly limiting its functionality as a power device substrate.

[0006] In addition, Patent Document 2 discloses + A method has been disclosed in which implanted single-crystal and polycrystalline SiC substrates are bonded together, and then the single-crystal and polycrystalline SiC substrates are delaminated separately. However, there are problems with the cost increase due to the two delamination steps, and with the difficulty of performing the delamination steps separately in the designated steps.

[0007] In Patent Document 3, attention is paid to impurity concentration and defect density, and a high resistance substrate with a low defect density is fabricated by H +A method of transferring using implantation is described. This method reduces defects present in the original substrate, but does not mention the substrate after peeling.

[0008] Furthermore, Patent Document 4 discloses + The document describes the technology that is the basis for substrate peeling by the method described above, and mentions the diffusion barrier (oxygen diffusion barrier) function, but does not mention anything about the substrate after peeling.

[0009] Furthermore, Patent Document 5 also describes a wide variety of substrates. + It describes a method for producing the semiconductor device by using the separation technique of the above, and describes a method for epitaxially growing InGaN after polishing or dry etching the surface, but does not describe how to handle the separation substrate.

[0010] Furthermore, Patent Document 6 describes a method in which a device is fabricated on a silicon carbide substrate, a protective film is formed, ions are implanted, the substrate is bonded to a support substrate, and then high-temperature annealing is performed, and the substrate is reused after separation, but again there is no description of how to handle the substrate after separation.

[0011] In addition, Patent Document 7 discloses H + This paper describes a method in which ions are implanted into single crystal SiC, polycrystalline SiC is formed on the opposite surface, annealed, and then the SiC is epitaxially grown after the ion-implanted surface is peeled off and the peeled surface is polished. + In the substrate technology using the above, no specific method for reusing the peeled substrate is mentioned.

[0012] Furthermore, H + As a method for forming a support substrate when ion implantation is performed and then peeled off, Patent Document 8 discloses a method for forming a support substrate by using H + Growth of polycrystalline SiC on the substrate after implantation at 1000-1600°C. + Growth by DLI-CVD (Direct Liquid Injection-CVD) on the substrate after injection. + Methods such as sintering onto a substrate after implantation and liquid deposition are disclosed.

[0013] This method is adopted because, as described in Patent Document 8, it is difficult to join SiC to SiC, and problems have been pointed out with joining via W or Mo due to the presence of metal.

[0014] However, in this way + After implantation, deposition on a support substrate at high temperature results in H + Peeling off of the implanted layer can occur during deposition, and H + The substrate itself having the implanted layer is exposed to high temperatures, which not only changes the crystallinity but also forms a polycrystalline layer on the side surface, hindering reuse.

[0015] Japanese Patent Laid-Open No. 11-003842 Japanese Patent Laid-Open No. 2016-018890 Japanese Patent Laid-Open No. 2014-022711 Japanese Patent Laid-Open No. 2007-329470 Special Publication No. 2013-513963 Japanese Patent Laid-Open No. 2022-140396 International Publication No. 2022 / 158085 Special Publication No. 2022-542224 Special Publication No. 2023-502571 Special Publication No. 2023-502572

[0016] H. Biard, W. Schwarzenbach, S. Odoul, I. Radu, A. Potier, M. Ferrato, E. Iwamuro, "Progress in High Performance and High Reliability of SiC MOSFETs," Proceedings of the Wide Bandgap Semiconductor Society Special Open Symposium, Wide Bandgap Semiconductor Society, 2022. Guajioty, "Tailored polycrystalline substrate for SmartSiC™ substrates enabling high performance power devices", ICSCRM2022, 2022; Suga, "Room temperature bonding by surface activation and its mechanism", Applied Physics, Japan Society of Applied Physics, 89(9), 2020. p. 498

[0017] Thus, 4H—SiC is expected to be used in high-voltage devices, but the high cost of the substrate is a problem, and the challenge is how to reduce the cost of the bulk substrate. +A technique has been proposed in which ion implantation is performed to peel off the substrate, but in this case, costs can be reduced by reusing the substrate after peeling (otherwise costs will remain high). For this reason, how to reuse the substrate after peeling (to make a high-quality substrate) is extremely important, and H + This is the fundamental technology that will enable the widespread adoption of substrate peeling technology that uses ions, etc.

[0018] On the other hand, H + After ion implantation and delamination of the substrate, the delamination surface of the delamination substrate is rough and must be planarized before re-bonding can be performed, and bonding of SiC to itself is difficult. In addition, it may be preferable to planarize the delamination surface of the SiC transferred to the support substrate by delamination before performing epitaxial growth or the like on the delamination surface.

[0019] However, since SiC is a highly hard and difficult-to-process material, the cost required to flatten the peeled surface by polishing such as CMP is high, which ultimately leads to a problem of high substrate manufacturing costs. + In the method of growing a support substrate after implantation, the support substrate may peel off during growth, or polycrystalline SiC may grow unintentionally on the original substrate, hindering reuse.

[0020] H + In the case of injection, as mentioned earlier, + After implantation, deposition on a support substrate at high temperature results in H + Peeling off of the implanted layer can occur during deposition, and H + The substrate itself having the implanted layer is exposed to high temperatures, which not only changes the crystallinity but also forms a polycrystalline layer on the side surface, hindering reuse.

[0021] The present invention has been made to solve the above problems, and aims to provide a semiconductor substrate manufacturing method that uses 4H—SiC delamination technology to manufacture semiconductor substrates at lower cost and with higher quality. Another aim of the present invention is to provide a semiconductor substrate and semiconductor device at lower cost and with higher quality.

[0022] The present invention relates to a method for manufacturing a SiC wafer made to achieve the above-mentioned object, and more specifically to a substrate delamination technology that utilizes ion implantation of silicon, carbon, and oxygen, and relates to bonding to a support substrate and reuse of the substrate after delamination, thereby providing a cheaper, higher-quality SiC substrate. Specifically, the present invention has been made to achieve the above-mentioned object, and provides a method for manufacturing a semiconductor substrate, comprising: an ion implantation step of implanting at least one of silicon, carbon, and oxygen ions into a surface of a 4H—SiC substrate to form an amorphous layer in the 4H—SiC substrate, in which silicon and carbon are amorphized; a bonding step of forming a thin film on at least one of the surface of the 4H—SiC substrate that has been subjected to the ion implantation step and a bonding surface of another support substrate, and bonding the 4H—SiC substrate and the support substrate via the thin film to obtain a bonded substrate; a delamination step of peeling the 4H—SiC substrate using the amorphous layer of the bonded substrate to separate the 4H—SiC substrate into a bonded substrate in which the surface layer of the 4H—SiC substrate has been transferred as a 4H—SiC layer onto the support substrate; and a delamination substrate, which is the substrate obtained after the surface layer has been delaminated from the 4H—SiC substrate; an etching step of plasma-etching the delamination surface of at least one of the bonded substrate and the delamination substrate after the delamination step; and an epitaxial step of performing epitaxial growth on at least one of the bonded substrate and the delamination substrate.

[0023] According to this method for manufacturing a semiconductor substrate, at least one of silicon, carbon, and oxygen ions are implanted into the surface of a 4H—SiC substrate to break the bond between silicon and carbon, thereby forming an amorphous layer. After bonding to a support substrate, the 4H—SiC substrate is peeled off from the amorphous layer, and the 4H—SiC layer is transferred to the bonded substrate.

[0024] In this way, in an ion implantation process using at least one of silicon, carbon, and oxygen ions, it is possible to inject damage to a predetermined depth by adjusting the acceleration energy during implantation. Specifically, the damage is the breaking of the bonds between silicon and carbon caused by the ion implantation of these ions. The broken silicon and carbon exist in an amorphous state.

[0025] The amorphous layer formed in this way can be peeled off by inserting a thin metal object from the side and applying an impact. Furthermore, since the amorphous layer becomes black due to the influence of carbon, it becomes more susceptible to absorbing light, so it can be further excited by irradiating it with light and peeled off. Alternatively, peeling can be achieved by combining light irradiation and impact.

[0026] In particular, when silicon or carbon is ion-implanted, such a delamination layer will not delaminate even when exposed to high temperatures, making it possible to carry out the delamination process at any time during the manufacturing process. Furthermore, when oxygen is ion-implanted, heat treatment can be applied to bond the implanted oxygen with the carbon in the amorphous layer, causing gasification, which also enables delamination.

[0027] In this way, in the present invention, bonding is performed after ion implantation of at least one of silicon, carbon, and oxygen. In this case, by using a polycrystalline body or a sintered body as the support substrate, as well as a single crystal, it is possible to significantly reduce costs.

[0028] It has also been reported that using a polycrystalline material is more effective in reducing the substrate resistance (Non-Patent Document 2), and is extremely effective in improving quality when considering vertical devices in addition to cost.

[0029] Then, a thin film of silicon or the like is sputtered onto the bonding surfaces of the substrate into which silicon or the like ions have been implanted and the support substrate, and bonding is performed via this thin film, making it possible to bond SiC substrates together, which are difficult to bond.

[0030] In particular, by preparing an inexpensive support substrate such as a polycrystalline material, forming a thin film of silicon or the like on the bonding surface, and bonding via the silicon or the like film, it becomes possible to bond SiC, which was previously difficult to bond when the support substrate was SiC.

[0031] Furthermore, in the present invention, the separated surface of at least one of the separated substrate and the bonded substrate is etched with plasma to remove damaged layers and flatten the surface before reuse or epitaxial growth. This allows SiC, a material that is difficult to process, to be flattened at a lower cost than polishing methods such as CMP, and makes it possible to obtain a high-quality substrate.

[0032] Although SiC is normally difficult to etch with plasma, it can be etched due to the weakening of the surface caused by ion implantation. If a single high-quality SiC substrate can be prepared by performing epitaxial growth using CVD in this manner, it becomes possible to inexpensively produce high-quality SiC substrates by repeatedly transferring the surface layer of the 4H—SiC substrate to a support substrate by repeating the ion implantation, bonding, peeling, etching, and epitaxial processes, and then repeatedly performing epitaxial growth using CVD.

[0033] In this case, in the peeling step, the amorphous layer is irradiated with light, subjected to an impact, or subjected to a combination of these treatments, thereby enabling the 4H—SiC substrate to be peeled off.

[0034] In this way, by irradiating the amorphous layer with light and allowing the amorphous layer to absorb the light, the energy required for peeling can be directly applied to the amorphous layer.

[0035] Furthermore, when the bonded substrate is peeled off by applying an impact to the amorphous layer, the peeling can be achieved simply by inserting, for example, a thin metal blade into the amorphous layer, which is advantageous in that the equipment required for peeling can be simplified.

[0036] Furthermore, by performing peeling using a combination of light irradiation and impact, the time required for peeling can be shortened compared to when either method is performed alone.

[0037] In this case, oxygen ions are implanted in the ion implantation step, and the 4H—SiC substrate can be separated in the peeling step by irradiating the amorphous layer with light, applying an impact, or performing heat treatment to cause the injected oxygen to react with carbon in the amorphous layer to generate gas, or by performing a combination of these processes.

[0038] By irradiating the amorphous layer with light in this way, the energy required for delamination can be directly applied to the amorphous layer. Also, when delaminating the bonded substrate by impacting the amorphous layer, delamination can be achieved by simply inserting a thin metal blade into the amorphous layer.

[0039] Furthermore, when oxygen ions are implanted during the ion implantation process, the implanted oxygen reacts with the carbon in the amorphous layer to generate gas, which can then be used for delamination using gas pressure. Therefore, delamination can be achieved by heating in addition to light irradiation and impact, broadening the options for delamination methods. Furthermore, combining these methods for delamination shortens the time required for delamination compared to using each method alone.

[0040] In this case, in the bonding step, a silicon thin film can be formed as the thin film, and bonding can be performed via this.

[0041] Since a silicon thin film is sometimes used as a base for epitaxial growth of 4H—SiC, it is easy to bond to 4H—SiC, and it is also easy to bond to polycrystalline or sintered SiC. Therefore, bonding is made easier by preparing a support substrate such as polycrystalline SiC, which is cheaper than single-crystal SiC, forming a thin layer of silicon on the bonding surface, and bonding via the silicon.

[0042] In this case, in the bonding step, the silicon thin film can be formed by sputtering using silicon as a target.

[0043] In this way, forming a silicon thin film by sputtering, which involves ionizing and irradiating an inert gas such as Ar onto a silicon target, is advantageous in terms of adhesion, etc. It has been found that the roughness of the bonding surface in this case is preferably 1 nm or less (Non-Patent Document 3). Furthermore, using the sputtering method does not require high-temperature processing of the substrate on which the film is to be formed, and does not roughen the SiC surface of the bonding surface.

[0044] In this case, a mixed gas of fluorocarbon gas and oxygen can be used as a source gas in the etching step.

[0045] A mixed gas of fluorocarbon gas and oxygen is a gas used for etching silicon and the like, and so using it as a source gas is advantageous in that it is not necessary to prepare a gas specifically for etching SiC.

[0046] In this case, after the peeling step and before the etching step, an annealing step can be performed in which the peeled surface of the bonded substrate or the peeled substrate to be subjected to the etching step is annealed at a temperature of 1000° C. or higher in a hydrogen atmosphere.

[0047] By performing hydrogen annealing before etching in this way, the uneven shape of the peeled surface that has become rough due to peeling is reformed by hydrogen annealing before etching, and is flattened to a certain extent, which makes it easier to improve the flatness of the peeled surface in the etching process.

[0048] In this case, in the etching step, the peeled surface of the bonded substrate may be plasma etched, and further, after the etching step, the epitaxial step may be performed on the etched peeled surface of the bonded substrate.

[0049] By growing an epitaxial layer on the etched, exfoliated surface of the bonded substrate in this manner, devices can be formed on the epitaxial layer, resulting in higher quality devices.

[0050] The present invention also provides a semiconductor substrate comprising a support substrate and a 4H—SiC layer bonded to a surface of the support substrate, wherein the support substrate is made of SiC, the 4H—SiC layer is bonded to the support substrate via a silicon thin film, and the surface is etched.

[0051] In such a semiconductor substrate, the surface of the 4H—SiC layer of the semiconductor substrate is etched, so the surface is flat and an epitaxial layer can be formed without performing expensive planarization processes such as CMP, resulting in a cheaper, higher quality product.

[0052] Furthermore, when the 4H—SiC layer is bonded to a SiC support substrate via a silicon thin film, the silicon thin film is sometimes used as a base when epitaxially growing 4H—SiC, and therefore the bond between the 4H—SiC and the support substrate is strong, and the bond can be maintained even when the support substrate is a polycrystalline or sintered SiC body. Therefore, the bond between the support substrate and the 4H—SiC layer is strong.

[0053] Furthermore, the present invention provides a semiconductor device comprising the semiconductor substrate described above. Since such a semiconductor device comprises the above-described semiconductor substrate, it is inexpensive, high-quality, and highly reliable.

[0054] As described above, according to the semiconductor substrate manufacturing method of the present invention, a 4H—SiC delamination technique can be used to manufacture a semiconductor substrate of higher quality at lower cost, thereby reducing the manufacturing cost of the substrate. Furthermore, according to the semiconductor substrate manufacturing method of the present invention, it is possible to effectively utilize the 4H—SiC substrate after the surface layer has been delaminate, thereby reducing the manufacturing cost of the semiconductor substrate. Furthermore, the semiconductor substrate of the present invention is of higher quality at lower cost. Furthermore, the semiconductor device of the present invention is of higher quality at lower cost.

[0055] 1A and 1B are schematic diagrams of a semiconductor substrate according to the present invention, and a flow diagram of a method for manufacturing a semiconductor substrate according to the present invention.

[0056] The present invention will be described in detail below, but the present invention is not limited thereto.

[0057] As described above, there has been a demand for a semiconductor substrate manufacturing method that can manufacture cheaper, higher quality semiconductor substrates using 4H—SiC delamination technology, reduce the manufacturing cost of substrates, cheaper, higher quality semiconductor substrates, and cheaper, higher quality semiconductor devices.

[0058] As a result of extensive research into the above-mentioned problems, the present inventors have discovered a method for manufacturing a 4H-SiC substrate, comprising the steps of: an ion implantation step of implanting at least one of silicon, carbon, and oxygen ions into a surface of a 4H-SiC substrate to form an amorphous layer in the 4H-SiC substrate by amorphizing the silicon and carbon; a bonding step of forming a thin film on at least one of the surface of the 4H-SiC substrate that has been subjected to the ion implantation step and a bonding surface of another support substrate, and bonding the 4H-SiC substrate via the thin film to obtain a bonded substrate; and a bonding step of peeling the 4H-SiC substrate at the amorphous layer of the bonded substrate to obtain the 4H-SiC substrate. The inventors have found that a lower-cost, higher-quality semiconductor substrate can be manufactured using 4H—SiC delamination technology by a method for manufacturing a semiconductor substrate, the method comprising: a delamination step of separating a bonded substrate in which the surface layer of a 4H—SiC film is transferred onto the support substrate as a 4H—SiC layer; and a delamination substrate, which is the substrate obtained after the surface layer has been delaminated from the 4H—SiC substrate; an etching step of plasma-etching the delamination surface of at least one of the bonded substrate or the delamination substrate after the delamination step; and an epitaxial step of performing epitaxial growth on at least one of the bonded substrate or the delamination substrate, thereby completing the present invention.

[0059] Furthermore, as a result of extensive research into the above-mentioned problems, the inventors have discovered that a semiconductor substrate comprising a support substrate and a 4H—SiC layer bonded to the surface of the support substrate, wherein the support substrate is SiC, the 4H—SiC layer is bonded to the support substrate via a silicon thin film, and the surface is etched, can provide a cheaper, higher quality semiconductor substrate, and have completed the present invention.

[0060] Furthermore, as a result of extensive research into the above-mentioned problems, the inventors discovered that a semiconductor device characterized by including the semiconductor substrate described above can provide a cheaper, higher quality semiconductor device, and thus completed the present invention.

[0061] Preferred embodiments of the present invention will now be described with reference to the drawings. First, the configuration of a semiconductor substrate 5 will be described with reference to Fig. 1. As shown in Fig. 1, the semiconductor substrate 5 according to the embodiment of the present invention includes a support substrate 3 and a 4H—SiC layer 1a bonded to the surface of the support substrate 3, with the 4H—SiC layer 1a bonded to the support substrate 3 via a thin film 7.

[0062] The support substrate 3 is a substrate that supports the 4H—SiC layer 1a via the thin film 7, and the material and dimensions can be selected appropriately as long as it has sufficient strength to support the 4H—SiC layer 1a and does not cause unintended reactions with the thin film 7. A specific example is bulk 4H—SiC, which is made of the same material as the 4H—SiC layer 1a, but in consideration of cost, a sintered SiC substrate or a polycrystalline SiC substrate, which is less expensive than bulk 4H—SiC, may also be used.

[0063] The 4H—SiC layer 1a is a single crystal layer of 4H—SiC and is bonded to the surface of a support substrate 3. For this bonding, a thin film 7 is formed on the bonding surfaces of the 4H—SiC layer 1a and the support substrate 3, and bonding via this thin film 7 enables a strong bond.

[0064] The thin film 7 is made of a material, such as a silicon thin film, that can be bonded to the 4H—SiC layer 1 a and the support substrate 3. In the following description, unless otherwise specified, the present invention will be described taking as an example a case where a silicon thin film is used as the thin film 7.

[0065] Furthermore, the 4H—SiC layer 1 a has an etched surface 25. Since the 4H—SiC layer 1 a has an etched surface 25, the surface 25 becomes flat, and an epitaxial layer can be formed without performing expensive flattening processes such as CMP, resulting in a cheaper, higher-quality semiconductor substrate 5.

[0066] The 4H—SiC layer 1 a may be a bulk 4H—SiC layer or an epitaxial layer of 4H—SiC, provided that it is a single crystal layer.

[0067] The minimum thickness of the 4H—SiC layer 1a should be such that it can maintain its shape as a layer, can form a device, and is not lost during etching, polishing, etc. On the other hand, the maximum thickness is, for example, a thickness that minimizes the amount of wasted material that is not used when forming a device. The thickness can be, for example, 0.01 μm to 400 μm.

[0068] Next, the configuration of the semiconductor device 6 will be described with reference to Fig. 1. The semiconductor device 6 shown in Fig. 1 includes a semiconductor substrate 5. A specific example of the semiconductor device 6 is one in which desired semiconductor devices are formed on the semiconductor substrate 5, particularly on the 4H-SiC layer 1a. Of course, the semiconductor device 6 can also be divided into chips by dicing.

[0069] By including the semiconductor device 6 in the semiconductor substrate 5 that is less expensive and of higher quality, the semiconductor device 6 also becomes less expensive, of higher quality, and highly reliable.

[0070] Next, an outline of the method for manufacturing a semiconductor substrate 5 of the present invention will be described with reference to Fig. 2. First, a 4H—SiC substrate 1 is prepared as shown in Fig. 2(a). Here, single-crystal bulk 4H—SiC is exemplified as the 4H—SiC substrate 1, but a 4H—SiC epitaxial substrate may also be used.

[0071] In this embodiment, the surface layer of the 4H—SiC substrate 1 is transferred to the support substrate 3, but the peeled substrate 11 finally formed after the transfer may be reused as the 4H—SiC substrate 1. These 4H—SiC substrates 1 are preferably those that have been subjected to epitaxial growth by CVD.

[0072] Next, ions of at least one of silicon, carbon, and oxygen are implanted into the 4H—SiC substrate 1 to break the bonds between silicon and carbon near the surface of the 4H—SiC substrate 1, forming an amorphous layer 2 in which silicon and carbon are both amorphous, as shown in FIG. 2(b) (ion implantation step).

[0073] By adjusting the acceleration energy of the ion implantation, it is possible to form an amorphous layer 2 in which the silicon and carbon are both amorphous and present at a predetermined depth. When oxygen ions are implanted, an amorphous layer 2 and a layer in which oxygen exists are formed.

[0074] The ion species to be implanted must be at least one of silicon, carbon, and oxygen, and multiple types of ions may be implanted. Moreover, the type of ion to be implanted, silicon, carbon, or oxygen, may be appropriately selected in consideration of the advantages of each.

[0075] For example, when silicon or carbon is ion-implanted, these elements are elements that make up SiC, so implantation is advantageous in that they do not become impurities. On the other hand, when oxygen is ion-implanted, the 4H—SiC substrate 1 can be peeled off by heating in a subsequent process, so there are more options for peeling methods.

[0076] The acceleration energy during ion implantation varies depending on the depth position where the amorphous layer 2 is formed. Specifically, the deeper the position in the depth direction, the greater the acceleration energy, which is, for example, about 200 keV.

[0077] The amount of ions to be implanted may be sufficient to form the amorphous layer 2. For example, 17 atoms / cm 2 That's about it.

[0078] 2(c), a substrate separate from the 4H—SiC substrate 1 is prepared as the support substrate 3. The support substrate 3 may be a single-crystal 4H—SiC substrate having the same structure as the 4H—SiC substrate 1, but considering the cost, it is preferable to use sintered SiC or polycrystalline SiC, for example.

[0079] Next, as shown in FIG. 2( d ), a thin film 7 such as a silicon thin film is formed on the surface 14 of the 4H—SiC substrate 1 that has been subjected to the ion implantation process of silicon or the like and on the bonding surface 8 of the support substrate 3, and then these are bonded together to obtain the bonded substrate 10 shown in FIG. 2( e ) (bonding process).

[0080] It is preferable to form a silicon thin film as the thin film 7 and perform bonding via this. A silicon thin film is sometimes used as a base when epitaxially growing 4H—SiC, so it is easy to bond to 4H—SiC, and it is also easy to bond to polycrystalline or sintered SiC. Therefore, by preparing a support substrate 3 such as polycrystalline SiC, which is cheaper than single-crystal SiC, forming a thin layer of silicon on the bonding surface 8, and bonding via silicon, it becomes possible to bond even SiC, which is difficult to bond.

[0081] A specific method for forming the thin film 7 is the sputtering method, which uses silicon as a target and irradiates Ar ions onto the target to form a film, which is effective because it does not require high-temperature heating of the substrate and does not roughen the SiC surface at the bonding surface.

[0082] Furthermore, the 4H—SiC substrate 1 and the support substrate 3 can be bonded together via the thin film 7 by room temperature bonding, for example.

[0083] Next, as shown in FIG. 2( f), the 4H—SiC substrate 1 is peeled off at the amorphous layer 2 of the bonded substrate 10, thereby separating the 4H—SiC substrate 1 into a bonded substrate 12 in which the surface layer of the 4H—SiC substrate 1 is transferred onto the support substrate 3 as a 4H—SiC layer 1 a, and a peeled substrate 11, which is the substrate obtained after the surface layer has been peeled off from the 4H—SiC substrate 1 (peeling step).

[0084] Specifically, in the peeling step, the amorphous layer 2 is irradiated with light, subjected to an impact, or subjected to a combination of these treatments, thereby enabling the 4H—SiC substrate 1 to be peeled off.

[0085] When light irradiation is performed, light is irradiated onto bonded substrate 10, and the light is absorbed by amorphous layer 2 of silicon and carbon formed in the ion implantation process. This serves as a starting point for peeling off 4H—SiC substrate 1, thereby separating bonded substrate 10 into bonded substrate 12, in which the surface layer of 4H—SiC substrate 1 is transferred onto support substrate 3 as 4H—SiC layer 1a, and peeled substrate 11, which is the substrate remaining after the surface layer has been peeled off from 4H—SiC substrate 1.

[0086] In this way, by irradiating the amorphous layer 2 with light and allowing the amorphous layer 2 to absorb the light, the energy required for peeling can be directly applied to the amorphous layer 2 .

[0087] The light source of the irradiated light is not particularly limited as long as it can impart to the amorphous layer 2 sufficient energy to peel off the 4H—SiC substrate 1 starting from the amorphous layer 2, and an example of such a light source is a YAG laser. When a YAG laser is used as the light source, the wavelength of the irradiated light can be the fundamental wavelength (1064 nm).

[0088] In the peeling step, when applying an impact to the amorphous layer 2, it is also possible to peel the amorphous layer 2 without irradiating it with light by simply inserting, for example, a thin metal blade into the amorphous layer 2. This method of peeling the amorphous layer 2 by applying an impact to it is advantageous in that the equipment required for peeling can be simplified.

[0089] Furthermore, the separation can be achieved by combining light irradiation and impact. Specifically, in addition to light irradiation, it is also possible to insert a thin metal blade or the like into the carbon amorphous layer 2 to apply impact and thereby separate the layer. In this case, the time required for separation can be shortened compared to when light irradiation or impact is applied alone.

[0090] If oxygen ions are implanted in the ion implantation step, the 4H—SiC substrate 1 can be delaminated in the delamination step by irradiating the amorphous layer 2 with light, applying an impact, or performing heat treatment to cause the implanted oxygen to react with the carbon in the amorphous layer to generate gas, or by performing a combination of these processes.

[0091] Since the separated surface 23 of the bonded substrate 12 obtained by this separation has a rough surface, it may be preferable to flatten the surface if an epitaxial layer is to be formed in a later process. Furthermore, by repeatedly reusing the separated substrate 11 through the ion implantation process, bonding process, and separation process, the surface layer can be transferred to a plurality of support substrates 3. However, since the separated surface 21 has a rough surface, it must be flattened in order to bond it to the support substrate 3. Therefore, the procedure for flattening the separated surfaces 23 and 21 will be described below.

[0092] First, as shown in FIG. 2(h), at least one of the peeled surface 23 of the bonded substrate 12 and the peeled surface 21 of the peeled substrate 11 after the peeling step is plasma etched (etching step).

[0093] 2 illustrates an example in which both the release surface 23 of the bonded substrate 12 and the release surface 21 of the release substrate 11 are etched, but it is also possible to etch only one of them. For example, if an epitaxial layer can be formed without planarizing the release surface 23 of the bonded substrate 12, or if the 4H—SiC layer 1a is an epitaxial layer and no further epitaxial layer needs to be formed, it is also possible to etch only the release surface 21 of the release substrate 11.

[0094] By plasma etching at least one of the separated surface 23 of the bonded substrate 12 and the separated surface 21 of the separated substrate 11, the surface of SiC, which is a material that is difficult to process, can be flattened at a lower cost than by CMP or the like.

[0095] A mixed gas of fluorocarbon gas and oxygen can be used as a source gas for etching. A specific example of the fluorocarbon gas is CHF 3 and CF 4 Since the mixed gas of fluorocarbon gas and oxygen is a gas used for etching silicon and the like, using it as a source gas is advantageous in that it is not necessary to prepare a gas specifically for etching SiC.

[0096] The plasma form during the etching process may be optimized depending on the device, and is not particularly limited, but may be RF plasma. Generally, SiC is not etched with a mixed gas of fluorocarbon gas and oxygen gas. However, the ion implantation process weakens the peeled surfaces 23 and 21, and the surface layer is a damaged layer. Therefore, the peeled surfaces 23 and 21 can be flattened by removing this layer by etching. Furthermore, the weakening is not only caused by damage due to ion implantation, but also by H 2 Plasma treatment using gas is also possible.

[0097] After the peeling step and before the etching step, the peeled surface 23 of the bonded substrate 12 or the peeled surface 21 of the peeled substrate 11 to be etched may be annealed in a hydrogen atmosphere at a temperature of 1000° C. or higher (annealing step), as shown in FIG. 2( g). The upper limit of the annealing temperature is not particularly limited, but may be 2000° C. or lower.

[0098] By performing hydrogen annealing in the annealing step before the etching step, the uneven shape of the peeled surface 23 or the peeled surface 21, which has been roughened by peeling, is reformed by hydrogen annealing before etching, and is flattened to some extent. Therefore, it becomes easier to improve the flatness of the peeled surface 23 or the peeled surface 21 in the etching step.

[0099] The exfoliated substrate 11 after the exfoliation process can be reused as a 4H—SiC substrate 1 by repeating the ion implantation process, bonding process, and exfoliation process again, until it becomes thick enough that it cannot be exfoliated any further, and can be used again as a substrate for transferring 4H—SiC to a support substrate 3.

[0100] Here, when the release surface 21 of the release substrate 11 is etched in an etching process, the release surface 21 is planarized by etching, so that the support substrate 3 can be bonded to the release surface 21 without performing costly planarization processing such as CMP.

[0101] Next, epitaxial growth is performed on at least one of the bonded substrate 12 and the separated substrate 11 (epitaxial step). Specifically, the epitaxial layer 4 may be grown by CVD or the like.

[0102] 2(i) illustrates an example in which a 4H—SiC epitaxial layer 4 is grown on a 4H—SiC layer 1a of a bonded substrate 12. Here, if a delamination surface 23 of the 4H—SiC layer 1a is etched in an etching process, the delamination surface 23 is planarized by etching, and therefore, an epitaxial layer 4 can be formed on the delamination surface 23 without performing costly planarization processes such as CMP, thereby enabling the bonded substrate 12 to be converted into a semiconductor substrate 5 at lower cost and with higher quality.

[0103] In addition, when the 4H—SiC layer 1 a is an epitaxial layer and the thickness of the transferred 4H—SiC layer 1 a is sufficient to form a device in a subsequent process, it is not necessarily necessary to perform the epitaxial process shown in FIG. 2( i).

[0104] On the other hand, if the 4H—SiC layer 1 a is not an epitaxial layer, or if the 4H—SiC layer 1 a is an epitaxial layer but its film thickness at the time of transfer in the peeling step is not thick enough to form a device, it is preferable to perform an epitaxial step on the bonded substrate 12. In this case, it is preferable to smooth the peeled surface 23 by an etching step before performing the epitaxial step on the bonded substrate 12.

[0105] Specifically, it is preferable to plasma-etch the peeled surface 23 of the bonded substrate 12 in the etching step as shown in FIG. 2( h), and then grow the epitaxial layer 4 on the etched peeled surface 23 of the bonded substrate 12 in the epitaxial step as shown in FIG. 2( i).

[0106] By growing the epitaxial layer 4 on the etched peeled surface 23 of the bonded substrate 12 in this manner, devices can be formed on the epitaxial layer 4, resulting in higher quality devices.

[0107] The present invention will be described in detail below with reference to examples, but is not limited thereto. An attempt was made to reuse the exfoliated substrate 11 as the 4H—SiC substrate 1 by performing the steps of implanting silicon, carbon, and oxygen ions into the 4H—SiC substrate 1, the bonding step (forming a silicon thin film and bonding), the peeling step, and the etching step, and then performing the ion implantation step and the bonding step again.

[0108] Example 1 First, a 4H—SiC single crystal substrate having a diameter of 200 mm, a thickness of 355 μm, an n-type, a resistivity of 10 Ω·cm, and an offset of 4° with respect to the (0001) plane was prepared as a 4H—SiC substrate 1. In the ion implantation step, silicon ions were implanted into the substrate at a density of 1×10 with an acceleration energy of 200 keV using an ion implanter. 17 atoms / cm 2 Injected.

[0109] Next, the following steps were carried out as the bonding process. First, a polycrystalline SiC substrate of the same diameter as the 4H—SiC substrate 1 was prepared as the support substrate 3, and Ar ions were irradiated onto the support substrate 3 using silicon as a target to form a silicon thin film as the thin film 7 on both the 4H—SiC substrate 1 and the support substrate 3 by sputtering. The thickness of the silicon thin film at this time was set to 20 nm. After this, the 4H—SiC substrate 1 and the support substrate 3 were bonded at room temperature via the silicon thin film to obtain a bonded substrate 10.

[0110] Following the bonding step, a YAG laser (wavelength 1064 nm) was used to irradiate and excite the amorphous layer 2 in a peeling step, and the bonded substrate 10 was separated into a bonded substrate 12 and a peeled substrate 11 .

[0111] This bonded substrate 12 is subjected to an epitaxial process using a hot wall CVD apparatus. 2 as a carrier gas, and SiH 4 , C 3 H 8 was used as a source gas to perform epitaxial growth of 4H—SiC to obtain a semiconductor substrate 5. The temperature at this time was 1600° C. and the pressure inside the furnace was 7 kPa.

[0112] In this way, the separation surface 21 of the separation substrate 11 formed when the semiconductor substrate 5 is obtained is etched using a source gas of CHF 3 and O 2 The resulting mixture was subjected to RF plasma etching at 100 sccm and 10 sccm, respectively, a pressure of 100 Torr (13332.2 Pa), and an RF power of 500 W.

[0113] When the peeled substrate 11 after the etching process was subjected to the silicon ion implantation process and bonding process again using the same flow, the support substrate 3 could be bonded to the peeled surface 21 of the peeled substrate 11, and a bonded substrate 10 could be obtained in the same manner.

[0114] Example 2 First, a 4H—SiC single crystal substrate having a diameter of 200 mm, a thickness of 355 μm, an n-type, a resistivity of 10 Ω·cm, and an offset of 4° with respect to the (0001) plane was prepared as the 4H—SiC substrate 1. In the ion implantation step, carbon ions were implanted into the substrate at a dose of 1.0×10 using an ion implanter at an acceleration energy of 200 keV. 17 atoms / cm 2 Injected.

[0115] Next, the following steps were carried out as the bonding process. First, a polycrystalline SiC substrate of the same diameter as the 4H—SiC substrate 1 was prepared as the support substrate 3, and Ar ions were irradiated onto the support substrate 3 using silicon as a target to form a silicon thin film 7 on both the 4H—SiC substrate 1 and the support substrate 3 by sputtering. The silicon thin film at this time was 20 nm thick. After this, the 4H—SiC substrate 1 and the support substrate 3 were bonded at room temperature via the silicon thin film to obtain a bonded substrate 10.

[0116] Following the bonding step, a YAG laser (wavelength 1064 nm) was used to irradiate and excite the amorphous layer 2 in a peeling step, and the bonded substrate 10 was separated into a bonded substrate 12 and a peeled substrate 11 .

[0117] This bonded substrate 12 is subjected to an epitaxial process using a hot wall CVD apparatus. 2 as a carrier gas, and SiH 4 , C 3 H 8 was used as a source gas to perform epitaxial growth of 4H—SiC to obtain a semiconductor substrate 5. The temperature at this time was 1600° C. and the pressure inside the furnace was 7 kPa.

[0118] In this way, the separation surface 21 of the separation substrate 11 formed when the semiconductor substrate 5 is obtained is etched using a source gas of CHF 3 and O 2 The resulting mixture was subjected to RF plasma etching at 100 sccm and 10 sccm, respectively, a pressure of 100 Torr (13332.2 Pa), and an RF power of 500 W.

[0119] When the peeled substrate 11 after the etching process was subjected to the carbon ion implantation process and bonding process again in the same reuse flow, the support substrate 3 could be bonded to the peeled surface 21 of the peeled substrate 11, and a bonded substrate 10 could be obtained in the same manner.

[0120] Example 3 First, a 4H—SiC single crystal substrate having a diameter of 200 mm, a thickness of 355 μm, an n-type, a resistivity of 10 Ω·cm, and an offset of 4° with respect to the (0001) plane was prepared as the 4H—SiC substrate 1. In the ion implantation step, oxygen ions were implanted into the substrate at a dose of 1.0×10 using an ion implanter at an acceleration energy of 200 keV. 17 atoms / cm 2 Injected.

[0121] Next, the following steps were carried out as the bonding process. First, a polycrystalline SiC substrate of the same diameter as the 4H—SiC substrate 1 was prepared as the support substrate 3, and Ar ions were irradiated onto the support substrate 3 using silicon as a target to form a silicon thin film 7 on both the 4H—SiC substrate 1 and the support substrate 3 by sputtering. The thickness of the silicon thin film at this time was set to 20 nm. After this, the 4H—SiC substrate 1 and the support substrate 3 were bonded at room temperature to obtain a bonded substrate 10 as the bonding process.

[0122] Following the bonding step, a YAG laser (wavelength 1064 nm) was used to irradiate and excite the amorphous layer 2 in a peeling step, and the bonded substrate 10 was separated into a bonded substrate 12 and a peeled substrate 11 .

[0123] This bonded substrate 12 is subjected to an epitaxial process using a hot wall CVD apparatus. 2 as a carrier gas, and SiH 4 , C 3 H 8 was used as a source gas to perform epitaxial growth of 4H—SiC to obtain a semiconductor substrate 5. The temperature at this time was 1600° C. and the pressure inside the furnace was 7 kPa.

[0124] In this way, the separation surface 21 of the separation substrate 11 formed when the semiconductor substrate 5 is obtained is etched using a source gas of CHF 3 and O 2The resulting mixture was subjected to RF plasma etching at 100 sccm and 10 sccm, respectively, a pressure of 100 Torr (13332.2 Pa), and an RF power of 500 W.

[0125] When the peeled substrate 11 after the etching process was subjected to the oxygen ion implantation process and bonding process again using the same flow, the support substrate 3 could be bonded to the peeled surface 21 of the peeled substrate 11, and a bonded substrate 10 could be obtained in the same manner.

[0126] As described above, according to the embodiment of the present invention, amorphous layer 2 is formed on 4H—SiC substrate 1 by ion implantation, and then support substrate 3 is bonded to 4H—SiC substrate 1 via thin film 7. 4H—SiC substrate 1 is then peeled off at amorphous layer 2, thereby obtaining bonded substrate 12 in which the surface layer of 4H—SiC substrate 1 is transferred onto support substrate 3 as 4H—SiC layer 1a. Furthermore, peeled substrate 11 can be reused as 4H—SiC substrate 1.

[0127] This specification includes the following aspects: [1]: A method for manufacturing a semiconductor substrate, comprising: an ion implantation step of implanting at least one of silicon, carbon, and oxygen ions into a surface of a 4H—SiC substrate to form an amorphous layer in the 4H—SiC substrate, in which silicon and carbon are amorphized; a bonding step of forming a thin film on at least one of the surface of the 4H—SiC substrate that has been implanted with the ion implantation step and a bonding surface of another support substrate, and bonding the 4H—SiC substrate and the support substrate via the thin film to obtain a bonded substrate; a delamination step of separating the 4H—SiC substrate using the amorphous layer of the bonded substrate to form a bonded substrate in which the surface layer of the 4H—SiC substrate has been transferred as a 4H—SiC layer onto the support substrate, and a delamination substrate, which is the substrate obtained after the surface layer has been delaminated from the 4H—SiC substrate; an etching step of plasma-etching the delamination surface of at least one of the bonded substrate and the delamination substrate after the delamination step; and an epitaxial step of performing epitaxial growth on at least one of the bonded substrate and the delamination substrate. [2]: The method for manufacturing a semiconductor substrate according to [1] above, wherein in the delamination step, the 4H—SiC substrate is delaminated by irradiating the amorphous layer with light, applying an impact, or performing a combination of these processes. [3]: The method for manufacturing a semiconductor substrate according to [1] above or [2] above, wherein in the ion implantation step, oxygen ions are implanted, and in the delamination step, the 4H—SiC substrate is delaminated by irradiating the amorphous layer with light, applying an impact, or performing a heat treatment to cause the implanted oxygen to react with carbon in the amorphous layer to generate gas, or performing a combination of these processes. [4]: ​​The method for manufacturing a semiconductor substrate according to any one of [1] to [3] above, wherein in the bonding step, a silicon thin film is formed as the thin film and bonding is performed via the thin film. [5]: The method for manufacturing a semiconductor substrate according to [4] above, wherein in the bonding step, the silicon thin film is formed by a sputtering method using a silicon target.[6]: A method for manufacturing a semiconductor substrate according to any one of [1] to [5], characterized in that a mixed gas of fluorocarbon gas and oxygen is used as a source gas in the etching step. [7]: A method for manufacturing a semiconductor substrate according to any one of [1] to [6], characterized in that, after the separation step and before the etching step, an annealing step is performed in which the separation surface of the bonded substrate or the separation substrate to be subjected to the etching step is annealed in a hydrogen atmosphere at a temperature of 1000°C or higher. [8]: A method for manufacturing a semiconductor substrate according to any one of [1] to [7], characterized in that, in the etching step, the separation surface of the bonded substrate is plasma etched, and further, after the etching step, the epitaxial step is performed on the etched separation surface of the bonded substrate. [9]: A semiconductor substrate comprising a support substrate and a 4H—SiC layer bonded to a surface of the support substrate, wherein the support substrate is SiC, and the 4H—SiC layer is bonded to the support substrate via a silicon thin film and has an etched surface.

[10] : A semiconductor device comprising the semiconductor substrate according to [9].

[0128] The present invention is not limited to the above-described embodiments. The above-described embodiments are merely examples, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and that exhibits similar effects is included within the technical scope of the present invention.

Claims

1. A method for manufacturing a semiconductor substrate, comprising: an ion implantation step of implanting at least one of ions of silicon, carbon and oxygen into a surface of a 4H-SiC substrate to form an amorphous layer in the 4H-SiC substrate by amorphizing silicon and carbon; a bonding step of forming a thin film on at least one of the surface of the 4H-SiC substrate subjected to the ion implantation step and a bonding surface of another support substrate, and bonding the substrate via the thin film to obtain a bonded substrate; a delamination step of peeling the 4H-SiC substrate using the amorphous layer of the bonded substrate to separate the 4H-SiC substrate into a bonded substrate in which the surface layer of the 4H-SiC substrate has been transferred as a 4H-SiC layer onto the support substrate, and a delamination substrate, which is the substrate remaining after the surface layer has been delaminate from the 4H-SiC substrate; an etching step of plasma etching the delamination surface of at least one of the bonded substrate or the delamination substrate after the delamination step; and an epitaxial step of performing epitaxial growth on at least one of the bonded substrate or the delamination substrate.

2. The method for producing a semiconductor substrate according to claim 1, wherein in the peeling step, the 4H-SiC substrate is peeled off by irradiating the amorphous layer with light, applying an impact, or performing a combination of these processes.

3. A method for manufacturing a semiconductor substrate according to claim 1, characterized in that in the ion implantation step, oxygen ions are implanted, and in the peeling step, the amorphous layer is irradiated with light, impacted, or heat-treated to cause a reaction between the injected oxygen and carbon in the amorphous layer to generate gas, or a combination of these processes is performed to peel off the 4H-SiC substrate.

4. The method for manufacturing a semiconductor substrate according to claim 1, wherein in the bonding step, a silicon thin film is formed as the thin film and bonding is carried out via the silicon thin film.

5. The method for producing a semiconductor substrate according to claim 4, wherein in the bonding step, the silicon thin film is formed by a sputtering method using silicon as a target.

6. The method for manufacturing a semiconductor substrate according to claim 1, wherein a mixed gas of fluorocarbon gas and oxygen is used as a source gas in the etching step.

7. The method for manufacturing a semiconductor substrate according to claim 1, further comprising the step of: performing an annealing step after the peeling step and before the etching step, in which the peeled surface of the bonded substrate or the peeled substrate to be subjected to the etching step is annealed at a temperature of 1000°C or higher in a hydrogen atmosphere.

8. A method for manufacturing a semiconductor substrate according to any one of claims 1 to 7, characterized in that in the etching step, the peeled surface of the bonded substrate is plasma etched, and further, after the etching step, the epitaxial step is performed on the etched peeled surface of the bonded substrate.

9. A semiconductor substrate comprising a support substrate and a 4H-SiC layer bonded to a surface of the support substrate, the support substrate being made of SiC, the 4H-SiC layer being bonded to the support substrate via a thin silicon film, and having an etched surface.

10. A semiconductor device comprising the semiconductor substrate according to claim 9.

Citation Information

Patent Citations

  • Substrate for semiconductor electronic element and manufacture thereof

    JP1999003842A

  • Semiconductor-on-insulator wafer, and manufacturing method thereof

    JP2007329470A

  • How to reuse circuit boards

    JP2013513963A

  • Compound semiconductor

    JP2014022711A

  • SiC WAFER MANUFACTURING METHOD, SiC SEMICONDUCTOR MANUFACTURING METHOD AND SILICON CARBIDE COMPOSITE SUBSTRATE