Microwell film for bioassay, method for producing same, and photosensitive resin composition for forming microwell film for bioassay

The microwell film with an amino-modified resin layer and specific photosensitive resin composition improves fluorescence observation and S/N ratios in bioassays, addressing the challenges of high-density microwell arrays by enabling visible light fluorescence and enhanced sensitivity.

WO2024204175A1PCT designated stage expired Publication Date: 2024-10-03ASAHI KASEI KOGYO KABUSHIKI KAISHA +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011910
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-26
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

High-density microwell arrays for bioassays face challenges in achieving good contrast due to decreased signal-to-noise (S/N) ratios, making it difficult to detect fluorescent signals effectively, especially when using substrates like 4-Methylumbelliferone, which requires excitation light in the near-ultraviolet range, posing safety hazards and requiring specialized optical systems.

Method used

A microwell film with a resin layer containing amino-modified (meth)acrylate resin, a photosensitive resin composition comprising polyfunctional (meth)acrylate, alkyl (meth)acrylate with an amino group, and a photopolymerization initiator, along with a nitrogen-containing vinyl monomer, to enhance fluorescence observation in the visible light range and improve S/N ratios.

Benefits of technology

The solution enables fluorescence observation in the visible light range, increases fluorescence intensity, and enhances the S/N ratio, achieving higher sensitivity and quantitative performance even with densely packed microwells, suitable for single molecule enzyme assays.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024011910_03102024_PF_FP_ABST
    Figure JP2024011910_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present disclosure provides: a microwell film for bioassay, the microwell film having a fluorescence adjustment function, enabling fluorescence observation in a visible light region even when, for example, a 4-MU producing substrate or the like is used, and having a high S / N ratio and improved quantitativity; a method for producing the microwell film for bioassay; and the like. A microwell film for bioassay according to the present disclosure is provided with at least a base material and a resin layer that is provided on one surface of the base material and that has a microwell on a surface thereof. The resin layer includes a modified (meth)acrylate resin having an amino group. In the modified (meth)acrylate resin, the molar ratio of the amino group to a (meth)acrylate unit is 0.010-0.500.
Need to check novelty before this filing date? Find Prior Art

Description

Micro-well film for bioassay, method for producing same, and photosensitive resin composition for forming micro-well film for bioassay

[0001] The present invention relates to a fine well film for bioassay, a method for producing the same, and a photosensitive resin composition for forming a fine well film for bioassay.

[0002] One technique for rapidly and sensitively detecting markers such as nucleic acids, proteins, viruses, and cells for the diagnosis of diseases and infectious diseases is the "single-molecule enzyme assay," in which target substances such as nucleic acids, proteins, viruses, and cells are encapsulated in microdroplets and detected by immunological techniques using labeled antibodies. This method allows detection of target substances with single-molecule sensitivity (see, for example, Patent Document 1).

[0003] As a bioassay substrate for use in such single-molecule enzyme assays, it has been investigated to arrange fine wells at a high density using a photoimprinting technique that uses a photosensitive resin composition (see, for example, Patent Document 2).

[0004] Furthermore, a bioassay fine well film having low autofluorescence characteristics is provided, which is composed of at least a substrate and a resin layer provided on a first main surface of the substrate and having fine wells on its surface, and the substrate and the resin layer have an absorption coefficient of 0.01 μm or less at each wavelength from 350 nm to 800 nm. -1 A fine well film for bioassays has been proposed (see, for example, Patent Document 3):

[0005] JP 2011-137830 A JP 2008-044283 A International Publication No. 2021-002388 A

[0006] To further increase the sensitivity of digital bioassays, it is necessary to arrange microwells on a substrate at a high density. However, as the density of microwells increases, the intensity ratio (S / N ratio) between the fluorescent signal (S) and the background noise (N) tends to decrease, leading to new challenges such as the inability to obtain fluorescent images with good contrast and reduced quantitative accuracy. Furthermore, when a single-molecule enzyme assay method that detects the target substance with single-molecule sensitivity is applied as a liquid-encapsulated bioassay, the S / N ratio tends to decrease even further.

[0007] On the other hand, depending on the fluorescent dye used and the digital bioassay conditions, excitation of the fluorescent dye hardly occurs with excitation light in the 360-400 nm range at the lower end of the visible light range, making fluorescence observation using excitation light in the visible light range impossible. For example, in a digital bioassay using a substrate that generates the fluorescent dye 4-methylumbelliferone (4-MU) through an enzymatic reaction (hereinafter referred to simply as a "4-MU-generating substrate"), the central excitation wavelength of 4-MU is approximately 320 nm at pH levels below 7.0. When the excitation wavelength is in the near-ultraviolet or ultraviolet range (less than 350 nm), the excitation light itself is harmful to the human body, and the emission of the excitation light is imperceptible to the human eye, making it extremely dangerous. Furthermore, many plastics and glass materials are transparent in the visible light range but exhibit extremely poor optical transparency in the near-ultraviolet or ultraviolet ranges. Therefore, special optical system designs are often required for excitation and fluorescence observation using light in the near-ultraviolet or ultraviolet ranges.

[0008] The present invention has been made in view of the above-mentioned problems, and aims to provide a fine well film for bioassays, which has a fluorescence adjustment function, enables fluorescence observation in the visible light region even when using, for example, a 4-MU generating substrate, has a high S / N ratio, and has improved quantitativeness, a method for producing the same, and a photosensitive resin composition for forming the fine well film for bioassays that can be used for the same.

[0009] The present inventors have conducted extensive research to solve the above problems and have surprisingly found that a fine well film for bioassays, in which fine wells are formed in a resin layer containing a specific amino-modified (meth)acrylate resin, can solve the above problems, thereby completing the present invention. That is, the present invention provides the following various specific embodiments.

[0010] [1] A fine well film for bioassays, comprising at least a substrate and a resin layer provided on one surface of the substrate and having fine wells on its surface, wherein the resin layer contains a modified (meth)acrylate resin having an amino group, and the molar ratio of the amino group to the (meth)acrylate unit in the modified (meth)acrylate resin is 0.010 to 0.500.

[0011] [2] The resin layer is a cured product of a photosensitive resin composition containing at least a polyfunctional (meth)acrylate, a (meth)acrylic acid alkyl ester having an amino group, and a photopolymerization initiator. [1] The fine well film for bioassays described.

[0012] [3] The fine well film for bioassay according to [2], wherein the photosensitive resin composition further contains a nitrogen-containing vinyl monomer.

[0013] [4] The fine well film for bioassay according to any one of [1] to [3], wherein the amino group contains an N-alkylamino group and / or an N,N-dialkylamino group.

[0014] [5] The fine well film for bioassay according to any one of [1] to [4], wherein the amino group comprises one selected from the group consisting of an N-methylamino group, an N-ethylamino group, an N,N-dimethylamino group, an N-methyl-N-ethylamino group, and an N,N-diethylamino group.

[0015] [6] The fine well film for bioassay according to any one of [1] to [5], wherein the substrate is a cyclic olefin resin film.

[0016] [7] The well density of the fine wells is 1 million / cm 2 The fine well film for bioassay according to any one of [1] to [6] above.

[0017] [8] The fine well film for bioassay according to any one of [1] to [7], which is for use in a single molecule enzyme assay method.

[0018] [9] A photosensitive resin composition for forming a fine well film for bioassay, comprising at least (A) a polyfunctional (meth)acrylate, (B) a (meth)acrylic acid alkyl ester, and (C) a photopolymerization initiator, wherein the (B) (meth)acrylic acid alkyl ester comprises a (meth)acrylic acid alkyl ester having an amino group, and the molar ratio of the amino group to the (meth)acrylate unit contained in the photosensitive resin composition is 0.010 to 0.500.

[0019]

[10] The content of the (A) polyfunctional (meth)acrylate is 50.0 to 90.0% by mass relative to the total amount of the photosensitive resin composition, The content of the (B) amino group-containing (meth)acrylic acid alkyl ester is 0.1 to 10.0% by mass relative to the total amount of the photosensitive resin composition, and The content of the (C) photopolymerization initiator is 0.5 to 10.0% by mass relative to the total amount of the photosensitive resin composition. The photosensitive resin composition for forming a fine well film for bioassays according to [9].

[0020]

[11] The photosensitive resin composition for forming a fine well film for bioassay according to [9] or

[10] , further comprising (D) a nitrogen-containing vinyl monomer.

[0021]

[12] The content ratio of the (D) nitrogen-containing vinyl monomer is 10.0 to 50.0 mass% with respect to the total amount of the photosensitive resin composition.

[11] The photosensitive resin composition for forming a fine well film for bioassay.

[0022]

[13] A method for producing a fine well film for bioassay according to [1], comprising the steps of: applying the photosensitive resin composition for forming a fine well film for bioassay according to [9] onto a substrate or a mold; pressing the photosensitive resin composition between the substrate and the mold; curing the photosensitive resin composition by exposure to light to obtain a cured product; and peeling off the cured product from the mold.

[0023]

[14] The method for producing a fine well film for bioassay according to

[13] , wherein the applying step applies the photosensitive resin composition to at least the substrate, and the method further includes a permeation step of permeating the photosensitive resin composition into the substrate before the pressing step.

[0024] According to the present invention, it is possible to realize a fine well film for bioassay, which has a fluorescence adjustment function, enables fluorescence observation using excitation light in the visible light region even when using a 4-MU-generating substrate, etc., has a high S / N ratio, and has improved quantitativeness, a method for producing the same, and a photosensitive resin composition for forming the fine well film for bioassay that can be used therefor.The fine well film for bioassay, etc. of the present invention is a novel material that achieves higher sensitivity than conventional materials even when the fine wells are highly dense, and can be used with single-molecule enzyme assays, etc., facilitating marker detection.

[0025] FIG. 1 is a perspective cross-sectional schematic diagram showing an overview of a bioassay microwell film 1 of one embodiment. FIG. 2 is a plan view schematic diagram showing an example of an arrangement of microwell recesses 13. FIG. 3 is a plan view schematic diagram showing another example of an arrangement of microwell recesses 13. FIG. 4 is a graph showing the excitation spectrum and fluorescence spectrum of 4-methylumbelliferone (4-MU) at pH 1 to 7. FIG. 5 is a graph showing the excitation spectrum and fluorescence spectrum of 4-methylumbelliferone (4-MU) at pH 7 to 10.5. FIG. 6 is a graph showing the excitation spectrum and fluorescence spectrum of 4-methylumbelliferone (4-MU) at pH 10.5 to 14.

[0026] Hereinafter, one embodiment for carrying out the present invention (hereinafter referred to as "the present embodiment") will be described in detail. Note that the following embodiment is an example for explaining the present invention, and the present invention is not limited thereto. In other words, the present invention can be carried out by making any modifications within the scope of the gist thereof. Note that in this specification, for example, when a numerical range is expressed as "1 to 100," it is intended to include both the lower limit "1" and the upper limit "100." The same applies to other numerical ranges.

[0027] In this specification, (meth)acrylate is used as a term that encompasses both acrylate and methacrylate, and (meth)acryloyl is used as a term that encompasses both acryloyl and methacryloyl.

[0028] 1 is a perspective cross-sectional schematic diagram showing a bioassay fine-well film 1 of this embodiment. The bioassay fine-well film 1 of this embodiment includes at least a substrate 11 and a resin layer 12 provided on one surface of the substrate 11 and having fine wells on its surface.

[0029] The bioassay micro-well film 1 of this embodiment is composed of a substrate 11 and a resin layer 12 having micro-wells, which allows the thickness of the entire well film to be thin and uniform within the plane. Furthermore, since the substrate 11 ensures uniformity in the thickness of the entire well film, the resin layer 12 having micro-wells only needs to be thick enough to form the micro-wells, which results in reduced thickness unevenness throughout the well film.

[0030] As mentioned above, the single-molecule enzyme assay method is an enzymatic reaction, and therefore is susceptible to the effects of the temperature environment. In particular, the so-called edge effect can be a problem, in which the reaction in the microwells located on the periphery of the substrate 11, when viewed from above, is affected by the ambient temperature and progresses (or slows) more rapidly than in the other microwells. Therefore, by thinning the entire well film as described above, uniform temperature control by the temperature control plate on the back side of the well film is facilitated, thereby suppressing the edge effect in the periphery of the substrate 11. Furthermore, since uneven thickness of the entire well film is suppressed, uneven temperature control tends to be further suppressed.

[0031] In particular, when the overall thickness of the well film is less than 300 μm, preferably less than 250 μm, the above-mentioned uniform temperature control of the well film becomes easy, and the effect of excellent in-plane uniformity tends to be obtained.

[0032] In the embodiment shown in FIG. 1 , the bioassay micro-well film 1 is in the form of a film and includes a substrate 11 and a resin layer 12 having micro-wells provided on one side of the substrate 11. The resin layer 12 includes recesses 13 (chambers) as multiple micro-wells extending in-plane from one side of the bioassay micro-well film 1 (toward the other side (back side) opposite to one side (front side)). The multiple recesses 13 are recessed in the thickness direction (Z-axis direction) perpendicular to one side F of the bioassay micro-well film 1, from the one side F toward the bottom in the figure (inside the bioassay micro-well film 1). The multiple recesses 13 are each arranged at a predetermined pitch. Each component is described in detail below.

[0033] <Substrate> The material of the substrate 11 is not particularly limited as long as it is suitable for the intended bioassay, and any material known in the art can be used, regardless of whether it is an inorganic material such as glass or ceramic, or an organic material such as plastic. From the viewpoints of productivity and handleability, a resin film that is flexible and has excellent continuous productivity is preferred. Laminated resin films in which a resin film is combined with a thin film, woven fabric, nonwoven fabric, etc. can also be used. The material of the resin film is not particularly limited, but preferred examples include polyethylene terephthalate, polycarbonate, cyclic olefin (cycloolefin polymer), polydimethylsiloxane, and polystyrene.

[0034] In particular, cyclic olefins are particularly preferred as resin films for the substrate 11 because they have excellent transparency from the ultraviolet to infrared regions and low autofluorescence in this wavelength range. This is because the substrate 11 for bioassays requires low autofluorescence, that is, low fluorescence emitted by the bioassay substrate itself, since fluorescence is used to detect markers such as nucleic acids, proteins, viruses, and cells. Known examples of such cyclic olefins include cycloolefin polymers (COP) and cycloolefin copolymers (COC), and examples of commercially available products include, but are not limited to, ZeonorFilm (registered trademark) manufactured by Zeon Corporation and ARTON (registered trademark) film manufactured by JSR Corporation.

[0035] The thickness of the substrate 11 in the bioassay microwell film 1 of this embodiment is not particularly limited as long as it can form a resin layer 12 having microwells on its surface. If the total thickness of the microwell film 1, including the surface resin layer 12, is thinner than the thinnest molded product obtained by conventional injection molding, well temperature control is easy, edge effect is suppressed, and autofluorescence characteristics can be suppressed, making marker detection easier. From this perspective, the thickness of the substrate 11 is preferably 300 μm or less, more preferably 200 μm or less, and even more preferably 190 μm or less. Furthermore, the lower limit of the thickness of the substrate 11 is not particularly limited, but from the viewpoints of handleability, well temperature control, edge effect, etc., it is preferably 10 μm or more, more preferably 30 μm or more, and even more preferably 50 μm or more.

[0036] <Resin Layer> The resin layer 12 of the bioassay fine well film 1 of this embodiment contains a modified (meth)acrylate resin having an amino group. Herein, the modified (meth)acrylate resin having an amino group refers to a so-called amino-modified (meth)acrylate resin in which an amino group has been introduced into a (meth)acrylate resin.

[0037] The (meth)acrylate resin contained in the resin layer 12 has an amino group, which is a weak anion exchange functional group, introduced therein, and thus the fluorescent dye having a tautomer in acid-base equilibrium is easily converted into H in the sample solution. + and OH - This allows the emission characteristics (excitation wavelength, fluorescence intensity) of the fluorescent dye to be changed.

[0038] More specifically, a digital bioassay using a 4-MU-generating substrate that generates the fluorescent dye 4-methylumbelliferone (4-MU) through an enzymatic reaction will be described in further detail. Figures 4 to 6 are graphs showing the excitation spectrum and fluorescence spectrum of 4-methylumbelliferone (4-MU) (quoted from Journal of Spectroscopy, Volume 2013 | Article ID 147128, "Fluorescent Properties of Hymecromone and Fluorimetric Analysis of Hymecromone in Compound Dantong Capsule"). 4-MU is known to have a tautomer represented by the following equilibrium formula: In this digital bioassay, the resin layer 12 contains a modified (meth)acrylate resin having an amino group, and the amino groups present on the surface of the resin layer 12 convert the H of 4-MU released into the sample solution. + or H in the solution 2 O to H + By removing the amino group, the equilibrium shift to Structure III in the following equilibrium equation is promoted. Furthermore, since the resin layer 12 contains a modified (meth)acrylate resin having an amino group, Structure III is easily adsorbed near the surface of the resin layer 12. Furthermore, as is clear from a comparison of Figures 5 and 4, the fluorescence intensity of 4-MU of Structure III, which has an excitation center wavelength of approximately 360 nm, is approximately 1.5 times higher than that of Structure I, which has an excitation center wavelength of approximately 320 nm. Therefore, this digital bioassay enables fluorescence observation in the visible light range, which was difficult with conventional digital bioassays performed in (meth)acrylate resins without amino groups (4-MU of Structure I), and also results in higher fluorescence intensity and an excellent S / N ratio. Furthermore, in this digital bioassay, fluorescence was observed on the wall surfaces of the recesses 13 of the microwells in the resin layer 12, suggesting that 4-MU of Structure III is adsorbed near the surface of the resin layer 12.

[0039] In this way, the modified (meth)acrylate resin having an amino group contained in the resin layer 12 has a fluorescence adjustment function that adjusts the emission characteristics (excitation wavelength, fluorescence intensity) of the fluorescent dye.As a result, even fluorescent dyes that were difficult to observe in the visible light range under the conventional digital bioassay conditions performed in (meth)acrylate resins that do not have amino groups can be observed in the visible light range, and it is possible to obtain higher fluorescence intensity, thereby increasing the S / N ratio.

[0040] The amino-group-containing modified (meth)acrylate resin of the resin layer 12 described above can be synthesized by methods known in the art, and the synthesis method is not particularly limited. For example, an amino-modified (meth)acrylate resin can be obtained by aminating or alkylaminating a (meth)acrylate resin. Alternatively, an amino-group-modified (meth)acrylate resin (copolymer) can be obtained by introducing a copolymerization component having an amino group during the synthesis of the (meth)acrylate resin. In a preferred embodiment, the amino-group-containing modified (meth)acrylate resin can be obtained as a cured product of a photosensitive resin composition containing at least a multifunctional (meth)acrylate, an amino-group-containing (meth)acrylic acid alkyl ester, and a photopolymerization initiator. Here, the photosensitive resin composition of this embodiment may be a radical polymerization system or a cationic polymerization system, but is not particularly limited thereto. A photopolymerizable radical polymerization photosensitive resin composition of this embodiment is preferred.

[0041] As the polyfunctional (meth)acrylate, one having a glass transition temperature after curing of preferably 100°C or higher, more preferably 120°C or higher can be used. Specifically, monomers having an acryloyl group or a methacryloyl group are more preferred. Here, the glass transition temperature after curing refers to the glass transition temperature of the cured product of the mixture of (meth)acrylates used. That is, for example, when (meth)acrylate A, (meth)acrylate B, and (meth)acrylate C are used, even if the glass transition temperatures of (meth)acrylates A, B, and C after curing are 60°C, 100°C, and 120°C, respectively, if the glass transition temperature of the mixture ((meth)acrylate A + (meth)acrylate B + (meth)acrylate C) after curing is 105°C, 105°C is adopted as the glass transition temperature.

[0042] The number of polymerizable groups in the polyfunctional (meth)acrylate is not particularly limited, but is preferably an integer of 2 to 6 from the viewpoint of polymerizability. Furthermore, when two or more types of polymerizable monomers are used in combination, the average number of polymerizable groups is preferably 2 to 5. When a single monomer is used, a polyfunctional (meth)acrylate having three or more polymerizable groups is preferred in order to increase the number of crosslinking points after the polymerization reaction and obtain physical stability (strength, heat resistance, etc.) of the cured product. Note that a monofunctional (meth)acrylate having one polymerizable group can also be used in combination as needed.

[0043] Specific examples of polyfunctional or monofunctional (meth)acrylates are not particularly limited, but include the following compounds: First, examples of monomers having an acryloyl group or a methacryloyl group include (meth)acrylic acid, aromatic (meth)acrylates [phenoxyethyl acrylate, benzyl acrylate, etc.], hydrocarbon (meth)acrylates [stearyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, allyl acrylate, 1,3-butanediol diacrylate, 1,4-butanediol diacrylate, 1,6-hexanediol diacrylate, trimethylolpropane triacrylate, pentaerythritol triacrylate, dipentaerythritol hexaacrylate, etc.], hydrocarbon (meth)acrylates containing an etheric oxygen atom [ethoxyethyl acrylate, methoxyethyl acrylate, glycidyl acrylate, tetrahydrofurfuryl acrylate, diethylene glycol diacrylate, neopentyl glycol diacrylate, polyoxyethylene glycol diacrylate, tripropylene glycol diacrylate, etc.], hydrocarbon (meth)acrylates containing a functional group [2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 4-hydroxybutyl vinyl ether, etc.].

[0044] Other examples include EO-modified glycerol tri(meth)acrylate, ECH-modified glycerol tri(meth)acrylate, PO-modified glycerol tri(meth)acrylate, pentaerythritol triacrylate, EO-modified phosphate triacrylate, trimethylolpropane tri(meth)acrylate, caprolactone-modified trimethylolpropane tri(meth)acrylate, PO-modified trimethylolpropane tri(meth)acrylate, tris(acryloxyethyl)isocyanurate, and EO-modified trimethylolpropane tri(meth)acrylate. , dipentaerythritol hexa(meth)acrylate, caprolactone-modified dipentaerythritol hexa(meth)acrylate, dipentaerythritol hydroxypenta(meth)acrylate, alkyl-modified dipentaerythritol penta(meth)acrylate, dipentaerythritol poly(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, alkyl-modified dipentaerythritol tri(meth)acrylate, pentaerythritol ethoxytetra(meth)acrylate, pentaerythritol tetra(meth)acrylate p) acrylate, diethylene glycol monoethyl ether (meth)acrylate, dimethylol dicyclopentane di(meth)acrylate, di(meth)acrylated isocyanurate, 1,3-butylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, EO-modified 1,6-hexanediol di(meth)acrylate, ECH-modified 1,6-hexanediol di(meth)acrylate, allyloxy polyethylene glycol acrylate, 1,9-nonanediol di(meth)acrylate, EO-modified bisphenone Bisphenol A di(meth)acrylate, PO-modified bisphenol A di(meth)acrylate, modified bisphenol A di(meth)acrylate, EO-modified bisphenol F di(meth)acrylate, ECH-modified hexahydrophthalic acid diacrylate, neopentyl glycol di(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, EO-modified neopentyl glycol diacrylate, PO-modified neopentyl glycol diacrylate, caprolactone-modified hydroxypivalic acid ester neopentyl glycol,Stearic acid modified pentaerythritol di(meth)acrylate, ECH modified propylene glycol di(meth)acrylate, ECH modified phthalic acid di(meth)acrylate, poly(ethylene glycol-tetramethylene glycol) di(meth)acrylate, poly(propylene glycol-tetramethylene glycol) di(meth)acrylate, polypropylene glycol di(meth)acrylate, silicone di(meth)acrylate, tetraethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, polyester ter(di)acrylate, polyethylene glycol di(meth)acrylate, dimethyloltricyclodecane di(meth)acrylate, neopentyl glycol modified trimethylolpropane di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, triglycerol di(meth)acrylate, EO modified tripropylene glycol di(meth)acrylate, divinylethylene urea, divinylpropylene urea, 2-ethyl-2-butylpropanediol acrylate, 2-ethylhexyl methylpropanediol xyl (meth)acrylate, 2-ethylhexyl carbitol (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, acrylic acid dimer, benzyl (meth)acrylate, butanediol mono(meth)acrylate, butoxyethyl (meth)acrylate, butyl (meth)acrylate, cetyl (meth)acrylate p) acrylate, EO-modified cresol (meth)acrylate, ethoxylated phenyl (meth)acrylate, ethyl (meth)acrylate, dipropylene glycol (meth)acrylate, isoamyl (meth)acrylate, isobutyl (meth)acrylate, isooctyl (meth)acrylate, cyclohexyl (meth)acrylate, dicyclopentanyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyloxyethyl (meth)acrylate, isomyristyl (meth)acrylate, lauryl (meth)acrylate,Methoxydipropylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, methoxytriethylene glycol (meth)acrylate, methyl (meth)acrylate, methoxytripropylene glycol (meth)acrylate, neopentyl glycol benzoate (meth)acrylate, nonylphenoxypolyethylene glycol (meth)acrylate, nonylphenoxypolypropylene glycol (meth)acrylate, octyl (meth)acrylate, paracumylphenoxyethylene glycol (meth)acrylate, ECH-modified phenoxy acrylate, phenoxydiethylene glycol (meth)acrylate, phenoxyhexaethylene glycol (meth)acrylate, Examples of the monomer include phenoxytetraethylene glycol (meth)acrylate, phenoxyethyl (meth)acrylate, polyethylene glycol (meth)acrylate, polyethylene glycol-polypropylene glycol (meth)acrylate, polypropylene glycol (meth)acrylate, stearyl (meth)acrylate, EO-modified succinic acid (meth)acrylate, tert-butyl (meth)acrylate, tribromophenyl (meth)acrylate, EO-modified tribromophenyl (meth)acrylate, tridodecyl (meth)acrylate, EO-modified isocyanuric acid di- and triacrylate, ε-caprolactone-modified tris(acryloxyethyl)isocyanurate, ditrimethylolpropane tetraacrylate, etc. Furthermore, examples of the monomer having an allyl group include p-isopropenylphenol, and examples of the monomer having a vinyl group include styrene, α-methylstyrene, acrylonitrile, and vinylcarbazole. In addition, EO-modified means ethylene oxide-modified, ECH-modified means epichlorohydrin-modified, and PO-modified means propylene oxide-modified.

[0045] Furthermore, for example, examples of bisphenol A-based compounds that can be used include dimethacrylates of polyalkylene glycols in which an average of 2 moles of propylene oxide and an average of 6 moles of ethylene oxide have been added to both ends of bisphenol A, dimethacrylates of polyethylene glycols in which an average of 5 moles of ethylene oxide have been added to both ends of bisphenol A (NK Ester BPE-500, manufactured by Shin-Nakamura Chemical Co., Ltd.), and dimethacrylates of polyethylene glycols in which an average of 2 moles of ethylene oxide have been added to both ends of bisphenol A (NK Ester BPE-200, manufactured by Shin-Nakamura Chemical Co., Ltd.). For example, 1,6-hexanediol di(meth)acrylate, 1,4-cyclohexanediol di(meth)acrylate, polypropylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, 2-di(p-hydroxyphenyl)propane di(meth)acrylate, glycerol tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, polyoxypropyl trimethylolpropane tri(meth)acrylate, polyoxyethyl trimethylolpropane triacrylate, pentaerythritol tetra(meth)acrylate, hydroxypropyl-β'-(acryloyloxy)propyl phthalate, phenoxy polyethylene glycol (meth)acrylate, nonylphenoxy polyethylene glycol (meth)acrylate, nonylphenoxy polyalkylene glycol (meth)acrylate, polypropylene glycol mono(meth)acrylate, and the like.

[0046] Examples of urethane compounds include urethane compounds obtained by reacting a diisocyanate compound such as hexamethylene diisocyanate, tolylene diisocyanate, or 2,2,4-trimethylhexamethylene diisocyanate with a compound having a hydroxyl group and a (meth)acrylic group in one molecule (2-hydroxypropyl acrylate, oligopropylene glycol monomethacrylate, etc.). Specific examples include a reaction product of hexamethylene diisocyanate with oligopropylene glycol monomethacrylate (manufactured by NOF Corporation, Blenmer-PP1000). These compounds may be used alone or in combination of two or more.

[0047] The content of the above-mentioned polyfunctional (meth)acrylate can be appropriately set depending on the desired performance, and is not particularly limited. It is preferably 50.0 to 90.0% by mass, more preferably 55.0 to 85.0% by mass, and even more preferably 60.0 to 80.0% by mass, relative to the total amount of the photosensitive resin composition. The content of the optional monofunctional (meth)acrylate can be appropriately set depending on the desired performance, and is not particularly limited. It is preferably 0.0 to 20.0% by mass, more preferably 0.0 to 15.0% by mass, and even more preferably 0.0 to 10.0% by mass. By having the content of the polyfunctional (meth)acrylate within the above range, it tends to be easier to obtain a fine well film 1 for bioassays that has low viscosity and sufficient curing hardness, a high S / N ratio, and improved quantitativeness.

[0048] An amino group-containing (meth)acrylic acid alkyl ester is an alkyl (meth)acrylic acid ester in which an amino group has been introduced. Examples of the alkyl (meth)acrylic acid ester include alkyl (meth)acrylic acid esters having 1 to 18 carbon atoms in the alkyl moiety. Specific examples of the alkyl (meth)acrylic acid esters having 1 to 18 carbon atoms in the alkyl moiety include, but are not limited to, methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, cyclohexyl (meth)acrylate, methylcyclohexyl (meth)acrylate, and dodecyl (meth)acrylate. These may be used alone or in combination of two or more.

[0049] The amino group is not particularly limited, but an N-alkylamino group or an N,N-dialkylamino group is preferred. The number of carbon atoms in the alkyl moiety is not particularly limited, but is preferably 1 to 4, more preferably 1 to 3, and even more preferably 1 to 2. Specific examples include an N-methylamino group, an N-ethylamino group, an N-propylamino group, an N-butylamino group, an N-methyl-N-ethylamino group, an N,N-dimethylamino group, an N,N-diethylamino group, an N,N-dipropylamino group, an N,N-dibutylamino group, a 2-methoxyethylamino group, a (2-methoxyethyl)methylamino group, a bis(2-methoxymethyl)amino group, an N,N-(2-ethoxymethyl)methylamino group, and a 3-methoxypropylamino group, but is not particularly limited to these. Among these, an N,N-dialkylamino group is preferred, and an N,N-dimethylamino group, an N-methyl-N-ethylamino group, and an N,N-diethylamino group are more preferred. These may be used alone or in combination of two or more.

[0050] The content of the (meth)acrylic acid alkyl ester having the amino group described above can be appropriately set according to the desired performance and is not particularly limited, but is preferably 0.1 to 10.0% by mass, more preferably 0.2 to 9.0% by mass, and even more preferably 0.3 to 8.0% by mass relative to the total amount of the photosensitive resin composition. When the content of the (meth)acrylic acid alkyl ester having an amino group is within the above range, it tends to be easier to obtain a fine well film 1 for bioassays that has low viscosity, sufficient cured hardness, a high S / N ratio, and improved quantitativeness.

[0051] The photopolymerization initiator is not particularly limited, and known photopolymerization initiators can be used, but it is preferable that the photopolymerization initiator has low light absorption at wavelengths from 350 nm to 800 nm. The photopolymerization initiator induces a radical reaction or an ionic reaction by light, and a photopolymerization initiator that induces a radical reaction is preferred. Examples of the photopolymerization initiator include, but are not particularly limited to, the following photopolymerization initiators:

[0052] Examples of the photopolymerization initiator include photopolymerization initiators having an oxime ester structure (hereinafter also referred to as "oxime-based photopolymerization initiators"), photopolymerization initiators having an α-aminoalkylphenone structure (hereinafter also referred to as "α-aminoalkylphenone-based photopolymerization initiators"), photopolymerization initiators having an α-hydroxyalkylphenone structure (hereinafter also referred to as "α-hydroxyalkylphenone-based polymerization initiators"), photopolymerization initiators having an acylphosphine oxide structure (hereinafter also referred to as "acylphosphine oxide-based photopolymerization initiators"), and photopolymerization initiators having an N-phenylglycine structure (hereinafter also referred to as "N-phenylglycine-based photopolymerization initiators"). These may be used alone or in combination of two or more.

[0053] Among these, when an α-hydroxyalkylphenone-based polymerization initiator is used, the absorption coefficient at each wavelength of 350 nm to 800 nm after curing is 0.01 μm. -1 The absorption coefficient at a wavelength of 300 nm is 0.02 μm or less. -1This is particularly preferable because the absorption coefficient at each wavelength from 300 nm to 800 nm is maximum at or below this value.

[0054] Commercially available photopolymerization initiators include 1-[4-(phenylthio)]-1,2-octanedione-2-(O-benzoyloxime) (trade name: IRGACURE (registered trademark) OXE-01, manufactured by BASF), 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethanone-1-(O-acetyloxime) (trade name: IRGACURE OXE-02, manufactured by BASF), 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone (trade name: Omnirad (registered trademark) 379EG, manufactured by IGM Resins B.V.), and 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one (trade name: Omnirad (registered trademark) 379EG, manufactured by IGM Resins B.V.). 907, manufactured by IGM Resins B.V.), 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)benzyl]phenyl}-2-methylpropan-1-one (trade name: Omnirad 127, manufactured by IGM Resins B.V.), 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1 (trade name: Omnirad 369, manufactured by IGM Resins B.V.), 2-hydroxy-2-methyl-1-phenylpropan-1-one (trade name: Omnirad 1173, manufactured by IGM Resins B.V.), 1-hydroxycyclohexyl phenyl ketone (trade name: Omnirad 184, manufactured by IGM Resins B.V.), BV), 2,2-dimethoxy-1,2-diphenylethan-1-one (trade name: Omnirad 651, manufactured by IGM Resins BV), and oxime ester-based (trade name: Lunar 6, manufactured by DKSH Japan Co., Ltd.).

[0055] The content of the photopolymerization initiator can be appropriately set depending on the desired performance and is not particularly limited, but is preferably 0.5 to 10.0 mass %, more preferably 1.0 to 9.0 mass %, relative to the total amount of the photosensitive resin composition. When the content of the photopolymerization initiator is within the above range, the absorption coefficient at each wavelength of 350 nm to 800 nm after curing is 0.01 μm -1 This makes it easier to obtain the fine well film for bioassay of this embodiment.

[0056] In this embodiment, the photosensitive resin composition constituting the resin layer 12 having microwells preferably further contains a nitrogen-containing vinyl monomer. Specific examples of the nitrogen-containing vinyl monomer include, but are not limited to, N-vinylformamide, N-vinylacetamide, N-vinylpyrrolidone, and N-vinylcaprolactam. Among these, N-vinylpyrrolidone is preferred. These may be used alone or in combination of two or more. By containing the nitrogen-containing vinyl monomer in the resin layer 12, the nitrogen-containing vinyl monomer penetrates into the interior of the substrate 11 from the interface with the resin layer 12 and polymerizes within the substrate 11, forming a molecular chain network with the surface resin layer 12. This generates strong interfacial adhesion, improving adhesion between the resin layer 12 having microwells and the substrate 11, while also maintaining low autofluorescence. Furthermore, containing the nitrogen-containing vinyl monomer is preferable because it also improves releasability from the mold after polymerization. In particular, when a cyclic olefin resin film is used as the substrate 11, which has excellent transparency and low autofluorescence properties and is suitable as a substrate for bioassays but has poor adhesion to photosensitive resins, the adhesion between the substrate 11 and the resin layer 12 is good, which is preferable.

[0057] The content of the nitrogen-containing vinyl monomer can be appropriately set according to the desired performance and is not particularly limited, but is preferably 5.0% by mass or more relative to the total amount of the photosensitive resin composition. Furthermore, by having a content of 50.0% by mass or less, it is possible to suppress the by-production of low-polymerization oligomers that bleed out from the polymer, and it is also possible to suppress excessive moisture absorption of the resin layer 12 having the fine wells, which is preferable because it improves the moisture resistance of the bioassay fine well film 1 of this embodiment. From the viewpoint of the above-mentioned adhesion improvement effect, the content of the nitrogen-containing vinyl monomer is more preferably 15.0% by mass or more and 45.0% by mass or less, and particularly preferably 20.0% by mass or more and 40.0% by mass or less.

[0058] In this embodiment, the photosensitive resin composition constituting the resin layer 12 having the fine wells may contain, as necessary, other photopolymerizable monomers in addition to the above-mentioned polyfunctional (meth)acrylate and (meth)acrylic acid alkyl ester having an amino group. Examples of such acrylates include the monofunctional (meth)acrylates mentioned above, as well as isobornyl acrylate, 4-hydroxybutyl acrylate, isobutyl acrylate, t-butyl acrylate, isooctyl acrylate, 2-methoxyethyl acrylate, methoxytriethylene glycol acrylate, 3-methoxybutyl acrylate, ethoxyethyl acrylate, butoxyethyl acrylate, ethoxydiethylene glycol acrylate, ethyl diglycol acrylate, cyclic trimethylolpropane formal monoacrylate, imide acrylate, isoamyl acrylate, ethoxylated succinic acid acrylate, trifluoroethyl acrylate, ω-carboxypolycaprolactone monoacrylate, methylphenoxyethyl acrylate, cyclohexyl acrylate, 4-t-butylcyclohexyl acrylate, caprolactone-modified tetrahydrofuran, Examples of the acrylates include, but are not limited to, methylfurfuryl acrylate, tribromophenyl acrylate, ethoxylated tribromophenyl acrylate, 2-phenoxyethyl acrylate, acryloylmorpholine, phenoxydiethylene glycol acrylate, 2-hydroxy-3-phenoxypropyl acrylate, 1,4-cyclohexanedimethanol monoacrylate, 2-(2-ethoxyethoxy)ethyl acrylate, diethylene glycol monobutyl ether acrylate, lauryl acrylate, isodecyl acrylate, 3,3,5-trimethylcyclohexanol acrylate, octyl / decyl acrylate, tridecyl acrylate, caprolactone acrylate, ethoxylated (4) nonylphenol acrylate, methoxypolyethylene glycol (350) monoacrylate, and methoxypolyethylene glycol (550) monoacrylate. These may be used alone or in combination of two or more.

[0059] In this embodiment, the photosensitive resin composition constituting the resin layer 12 having the fine wells may contain, as necessary, other photopolymerizable oligomers in addition to the above-described polyfunctional (meth)acrylate and (meth)acrylic acid alkyl ester having an amino group. Examples of other photopolymerizable oligomers that can be used include, for example, photopolymerizable oligomers having an ethylenically unsaturated double bond. Examples of such oligomers include, but are not limited to, aromatic urethane oligomers, aliphatic urethane oligomers, epoxy acrylate oligomers, polyester acrylate oligomers, aliphatic urethane acrylate oligomers, and other special oligomers.

[0060] Commercially available products of these include UV-2000B, UV-2750B, UV-3000B, UV-3010B, UV-3200B, UV-3300B, UV-3700B, UV-6640B, UV-8630B, UV-7000B, UV-7610B, UV-1700B, UV-7630B, UV-6300B, UV-6640B, UV-7550B, UV-7600B, UV-7605B, UV-7610B, UV-7630B, UV-7640B, UV-7650B, UT-5449, and UT-5454 manufactured by Nippon Chemical Synthetic Co., Ltd.; CN902 manufactured by Sartomer Corporation; CN902J75, CN929, CN940, CN944, CN944B85, CN959, CN961E75, CN961H81, CN 962, CN963, CN963A80, CN963B80, CN963E75, CN963E80, CN963J85, CN964, C N965, CN965A80, CN966, CN966A80, CN966B85, CN966H90, CN966J75, CN968, CN969, CN970, CN970A60, CN970E60, CN971, CN971A80, CN971J75, CN972, CN9 73, CN973A80, CN973H85, CN973J75, CN975, CN977, CN977C70, CN978, CN980 , CN981, CN981A75, CN981B88, CN982, CN982A75, CN982B88, CN982E75, CN98 3, CN984, CN985, CN985B88, CN986, CN989, CN991, CN992, CN994, CN996, CN9 97, CN999, CN9001, CN9002, CN9004, CN9005, CN9006, CN9007, CN9008, CN900 9, CN9010, CN9011, CN9013, CN9018, CN9019, CN9024, CN9025, CN9026, CN9028, CN9029, CN9030, CN9060, CN9165, CN9167, CN9178, CN9290, CN9782, CN9783, CN9788, CN9893, EBECRYL (registered trademark) 210, EBECRYL 220, EBECRYL 230, EBECRYL 270, KRM8200, EBECRYL 5129, EBECRYL 8210, EBECRYL 8301 manufactured by Daicel-Cytec Co., Ltd.Examples of the photopolymerizable oligomers include, but are not limited to, EBECRYL8804, EBECRYL8807, EBECRYL9260, KRM7735, KRM8296, KRM8452, EBECRYL4858, EBECRYL8402, EBECRYL9270, EBECRYL8311, and EBECRYL8701. These may be used alone or in combination of two or more. Synthesized photopolymerizable oligomers may also be used alone or in combination.

[0061] The amount of the photopolymerizable oligomer is preferably 1 to 45% by mass, more preferably 3 to 30% by mass, based on the weight of the photosensitive resin composition. This range can suppress unevenness in the thickness of the cured product obtained in the photoimprinting method, and can produce a fine well film for bioassays having fine wells suitable for the "single-molecule enzyme assay" method by the photonanoimprinting method.

[0062] In the amino-modified (meth)acrylate resin, the molar ratio of amino groups to (meth)acrylate units is 0.010 to 0.500. The molar ratio is preferably 0.012 to 0.450, and more preferably 0.015 to 0.400. When the introduction ratio of amino groups is within the above range, a fluorescence adjustment function is exhibited, and fluorescence observation in the visible light region and higher fluorescence intensity tend to be obtained.

[0063] The molar ratio of amino groups to (meth)acrylate units can be calculated based on the amounts of raw materials used in the photosensitive composition when they are known. For example, when a polyfunctional (meth)acrylate and a monofunctional (meth)acrylate are used in combination, the ratio is calculated as follows. That is, the molar ratio of (meth)acrylate units is calculated as the number of moles of (meth)acrylate units in the polyfunctional (meth)acrylate (for example, in the case of a trifunctional (meth)acrylate, this is calculated as "×3 moles"), the number of moles of (meth)acrylate units in the monofunctional (meth)acrylate (for example, in the case of a (meth)acrylate, this is calculated as "×1 mole"), and the number of moles of (meth)acrylate units in the (meth)acrylate alkyl ester having an amino group (for example, in the case of a (meth)acrylate alkyl ester having an N,N-dialkylamino group, this is calculated as "×1 mole"). Here, the number of moles of amino groups is calculated according to the number of moles corresponding to the substitution number of amino groups in the (meth)acrylic acid alkyl ester having amino groups. For example, when the amino group is monosubstituted, the calculation is made as "×1 mole," and when the amino group is disubstituted, the calculation is made as "×2 moles."

[0064] In this embodiment, the microwells are not particularly limited as long as they are micro-recessed structures suitable for the intended bioassay, but it is preferable that the recesses 13 have hole structures. The cross-sectional shape of the recesses 13 with hole structures is not particularly limited, but may be rectangular, square, trapezoidal, or shapes with curvature at the corners thereof, or circular. The top planar shape of the recesses 13 with hole structures may be rectangular, square, trapezoidal, rhombic, hexagonal, triangular, or shapes with curvature at the corners thereof, or circular.

[0065] Furthermore, the pattern arrangement of these recesses 13 is appropriately selected depending on the application and is not particularly limited. For example, the recesses 13 may be arranged randomly and substantially uniformly within the surface, or the recesses 13 may be arranged periodically. In particular, a pattern in which the recesses 13 having a hole structure are arranged periodically to form an array is preferred because it facilitates detection of a target substance in the "single-molecule enzyme assay" method.

[0066] 2 is a schematic plan view showing an example of the bioassay micro-well film 1 of this embodiment. As shown in FIG. 2, the recesses 13 formed on one surface of the resin layer 12 containing the micro-wells are arranged at regular intervals with the same pitch, forming a four-sided configuration.

[0067] 3 is a schematic plan view showing another example of the bioassay microwell film 1 of this embodiment. As shown in FIG. 3, the recesses 13 formed on one surface of the resin layer 12 containing the microwells are arranged at regular intervals with the same pitch, forming a three-sided configuration.

[0068] In this embodiment, the size of the recess 13 of the hole structure is not particularly limited, as long as it is selected to be a size appropriate for the bioassay to be used. For example, if the top planar shape of the hole structure is circular, its diameter is preferably in the range of 50 nm to 100 μm, and a diameter in the range of 100 nm to 50 μm is more preferable as it is suitable for bioassays such as RNA and cell detection. Furthermore, a diameter in the range of 200 nm to 10 μm is particularly preferable as it is optimal for "single-molecule enzyme assays."

[0069] The depth (maximum depth) of the recess 13 of the hole structure is not particularly limited and is selected to be a size suitable for the bioassay to be used. For example, a range of 50 nm to 100 μm is preferable, and a diameter range of 100 nm to 50 μm is more preferable since it is suitable for bioassays for the same reasons as above. Furthermore, a range of 200 nm to 10 μm is particularly preferable since it is optimal for "single-molecule enzyme assays" as described above.

[0070] The pitch between the recesses 13 in this embodiment is not particularly limited and is selected to be a size suitable for the intended bioassay. For example, a range of 200 nm to 400 μm is preferable, a range of 400 nm to 200 μm is preferable because it facilitates detection of the target substance in the bioassay, and a range of 800 nm to 40 μm is particularly preferable because it maximizes detection sensitivity in a "single-molecule enzyme assay."

[0071] In this specification, the pitch between each recess 13 is the shortest distance between the centers of each hole and the other hole closest to it, and in a pattern shape in which each recess 13 is periodically arranged, it is the periodic pitch, and in the case in which each recess 13 is randomly arranged, it is the average value of the individual closest distances.

[0072] The well density of each recess 13 of the micro-well of this embodiment can be appropriately set depending on the desired performance, and is not particularly limited. However, from the viewpoint of detection sensitivity in the "single molecule enzyme assay," it is set to 1 million / cm in plan view of the resin layer 12. 2 Preferably, the density is 1.5 million particles / cm or more, and more preferably, 1.5 million particles / cm 2 More preferably, 2 million particles / cm 2 That's all.

[0073] The thickness of the resin layer 12 having the microwells in this embodiment is not particularly limited as long as it can form the resin layer 12 having the microwells on its surface. For example, the thickness of the thinnest part of the well bottom is preferably in the range of 1 nm to 10 μm, and more preferably 10 nm to 1 μm from the viewpoint of suppressing uneven temperature control of the microwell film. Here, the thickness of the thinnest part of the well bottom of the resin layer 12 can be measured, for example, by observation with a scanning electron microscope (hereinafter referred to as SEM). Specifically, first, a sample is cut to an appropriate size, then cleaved at room temperature and placed on a sample stage. Next, the observation surface is coated with approximately 2 nm of Os to prepare a sample for microscopic examination, which can be measured using the apparatus and microscopic conditions shown below. Apparatus: HITACHI s-5500 Acceleration voltage: 10 kV MODE: Normal

[0074] <Absorption Coefficient> In the bioassay fine well film 1 of this embodiment, the substrate 11 and the resin layer 12 including the fine wells have an absorption coefficient of 0.01 μm at each wavelength from 350 nm to 800 nm. -1 It is preferable that the absorption coefficient at each wavelength is 0.01 μm or less. -1By suppressing the absorption coefficient to the following value, a fine well film with low autofluorescence characteristics in the wavelength range of 350 nm to 800 nm can be realized. Fluorescence is a phenomenon in which a substance absorbs excitation light of a specific wavelength and emits light with a longer wavelength than the excitation light due to the energy of the absorbed light. Therefore, suppressing the absorption coefficient tends to suppress the autofluorescence of the substrate and resin layer.

[0075] In this specification, the term "absorption coefficient" is determined by the following formula (1): Absorption coefficient = absorbance / film thickness (μm) Formula (1)

[0076] Furthermore, the absorbance is calculated according to the following formula (2): Absorbance = - log (light transmittance) Formula (2) The light transmittance is determined by measurement using a general spectrophotometric system, such as a spectrophotometer UV-2500 (manufactured by Shimadzu Corporation).

[0077] <<Method of Manufacturing a Micro-Well Film for Bioassay>> The method of manufacturing the micro-well film for bioassay 1 of this embodiment is not particularly limited, but a manufacturing method using a transfer method by photoimprinting from a predetermined mold (master mold, replica mold) can be applied. The master mold or replica mold is a metal mold for photoimprinting that has a reversed shape pattern of the desired micro-wells on its surface. Materials for the mold include quartz glass, ultraviolet-transmitting glass, sapphire, diamond, silicone materials such as polydimethylsiloxane, fluororesin, silicon, SiO 2 Examples of the material include, but are not limited to, Al, SiC, nickel, and chromium. Furthermore, each material may be laminated to form a composite. Furthermore, in order to improve the releasability during transfer, a release treatment known in the art may be performed.

[0078] From the viewpoint of the durability of the release treatment, a silane coupling type release agent is preferred as the release treatment agent. Examples of commercially available release agents include, but are not limited to, Optool DSX, Durasurf HD1100 and HD2100 manufactured by Daikin Industries, Ltd., and Novec manufactured by Sumitomo 3M Limited. These may be used alone or in combination of two or more.

[0079] Hereinafter, a preferred embodiment of the method for producing the fine well film 1 for bioassay of this embodiment will be described in order of each step.

[0080] <Step 1> Step 1: A photosensitive resin composition is applied onto a substrate 11 or a mold. The method for applying the photosensitive resin composition is not particularly limited, and known methods can be used. Examples include, but are not limited to, a casting method, a potting method, a spin coating method, a roller coating method, a bar coating method, a casting method, a dip coating method, a die coating method, a Langmuir-Blodgett method, a spray coating method, an air knife coating method, a flow coating method, and a curtain coating method. In this case, the coating thickness of the photosensitive resin composition can be appropriately set depending on the desired performance, and is not particularly limited, but is preferably 50 nm to 5 mm, more preferably 100 nm to 200 μm, and even more preferably 100 nm to 100 μm.

[0081] If the substrate 11 is larger than the mold (master mold, replica mold), the photosensitive resin composition may be applied to the entire surface of the substrate 11, or may be applied to a portion of the substrate 11 so that the photosensitive resin composition is present only in the area where the mold is to be embossed. Alternatively, the photosensitive resin composition may be applied to the mold side. Here, by applying the resin composition to the substrate 11 and then pre-baking, it is possible to remove the solvent (if present) or promote surface segregation of the (meth)acrylic acid alkyl ester having an amino group. By segregating the (meth)acrylic acid alkyl ester having an amino group to the surface, the amino group is unevenly distributed on the wall surface (surface) of the fine wells of the resulting resin layer 12, thereby enabling the development of a fluorescence-adjusting function. The treatment temperature can be set appropriately depending on the desired performance and is not particularly limited, but is preferably 25°C to 120°C, more preferably 40°C to 105°C, even more preferably 50°C to 105°C, and most preferably 60°C to 105°C. The treatment time can also be set appropriately depending on the desired performance, and is not particularly limited, but is preferably 30 seconds to 30 minutes, more preferably 1 minute to 15 minutes, and even more preferably 3 minutes to 10 minutes.

[0082] It is also preferable to apply a treatment for improving the adhesion between the substrate 11 and the photosensitive resin composition. For example, it is preferable to apply an easy-adhesion coating for chemical bonding with the photosensitive resin composition or physical bonding such as penetration, a primer treatment, a corona treatment, a plasma treatment, a UV / ozone treatment, a high-energy ray irradiation treatment, a surface roughening treatment, a porous treatment, or the like to the surface of the substrate 11 to be bonded.

[0083] <Step 2> Step 2: Penetration step of the photosensitive resin composition into the substrate 11 After applying the photosensitive resin composition to the substrate 11, it is preferable to provide a penetration step of the photosensitive resin composition into the substrate 11 in order to improve the adhesion between the cured photosensitive resin composition and the substrate 11. In the penetration step of this embodiment, it is sufficient that the photosensitive resin composition penetrates slightly into the interior near the surface of the substrate 11. For example, a method in which the photosensitive resin composition is applied to the substrate 11 and then left for a predetermined time can be mentioned. The conditions for the penetration step can be set appropriately depending on the desired performance and are not particularly limited, but the treatment temperature is preferably 15°C to 120°C, more preferably 20°C to 105°C, and even more preferably 25°C to 105°C. The processing time for the penetration step can be appropriately set depending on the desired performance and is not particularly limited, but is preferably 1 to 30 minutes, and 2 to 15 minutes is preferable because the adhesion of the photosensitive resin composition after curing is good, and 3 to 10 minutes is even more preferable because it can suppress an increase in haze at the interface with the substrate 11. In particular, by applying a photosensitive resin composition containing a nitrogen-containing vinyl monomer to the substrate 11 and allowing it to penetrate, the adhesive strength at the interface between the substrate 11 and the resin layer 12 can be effectively improved.

[0084] <Step 3> Step 3: Step of pressing the photosensitive resin composition between the substrate 11 and the mold It is preferable to gently coat the substrate 11, which has a relatively high flexibility, on the mold from the edge so as to prevent air bubbles from being trapped, and press the composition under a constant pressure. The pressing pressure can be appropriately set depending on the desired performance and is not particularly limited, but is preferably more than 0 MPa to 10 MPa, more preferably 0.01 MPa to 5 MPa, and even more preferably 0.01 MPa to 1 MPa.

[0085] <Step 4> Step 4: A step of curing the photosensitive resin composition by exposure to obtain a cured product. When the mold has low light transmittance, exposure is preferably performed from the substrate 11 side. On the other hand, when a mold with high transmittance to ultraviolet wavelength light is used, for example, when made of synthetic quartz, exposure is preferably performed from at least one side of the substrate 11 side or the mold side, and exposure from both the substrate 11 side and the mold side is more preferable. The atmosphere during exposure can be appropriately set depending on the desired performance and is not particularly limited, but may be a nitrogen atmosphere or argon atmosphere to prevent polymerization inhibition by oxygen.

[0086] The exposure light source used can be appropriately set depending on the desired performance and is not particularly limited, but metal halide lamps, high-pressure mercury lamps, chemical lamps, UV-LEDs, etc. are preferred. In this case, from the viewpoint of suppressing heat generation during long-term exposure, it is preferable to use a filter (including a bandpass filter) that cuts wavelengths longer than the visible wavelength. The integrated light amount can be appropriately set depending on the desired performance and is not particularly limited, but is preferably 300 mJ / cm at a wavelength of 365 nm. 2 The above is preferable, and from the viewpoint of obtaining a cured product with a high reaction rate, 800 mJ / cm 2 More preferably, 800 mJ / cm or more 2 ~6000mJ / cm 2 is more preferable, and in order to prevent deterioration of the resin due to light, 800 mJ / cm 2 ~3000mJ / cm 2 is particularly preferred.

[0087] Regardless of the thickness of the cured product, the total light transmittance of the cured product at 350 nm to 450 nm is preferably 50% or more, and for efficient photoreaction, it is more preferably 70% or more. When the thickness of the cured product is more than 0 nm to 50 μm, the total light transmittance of the cured product at 350 nm to 450 nm is preferably 50% or more, and more preferably 70% or more.

[0088] <Step 5> Step 5: Step of Peeling the Cured Product from the Mold When the mold is flexible, it is preferable to peel the cured product from at least one of the mold surface side or the substrate surface side at a constant speed. Linear peeling is a preferred peeling method. For example, when the mold is made of a highly rigid material, particularly an inorganic material, peeling from the mold side results in a large peeled area due to partial surface peeling, raising concerns about damage to the cured product. Therefore, peeling from the flexible substrate 11 side is preferred. The peeling speed can be set appropriately depending on the desired performance and is not particularly limited, but linear peeling from one direction at a constant speed of more than 0 m / min to 5 m / min is preferred in terms of reducing the risk of damage to the cured product.

[0089] It is also preferable to perform a heat treatment after curing and before peeling. By performing a heat treatment during this process, the number of unreacted groups in the cured product (photosensitive resin composition) can be reduced, making demolding easier and improving the durability of the mold. At this time, the treatment temperature can be set appropriately depending on the desired performance and is not particularly limited, but is preferably 50°C to 120°C, more preferably 50°C to 105°C, and even more preferably 60°C to 105°C. Furthermore, the treatment time can be set appropriately depending on the desired performance and is not particularly limited, but is preferably 30 seconds to 30 minutes, more preferably 30 seconds to 15 minutes, and even more preferably 1 minute to 10 minutes.

[0090] On the other hand, heat treatment may be performed after peeling. By performing heat treatment after peeling, the reaction of unreacted groups in the cured product (photosensitive resin composition) is promoted, which is preferable. At this time, the treatment temperature can be appropriately set depending on the desired performance and is not particularly limited, but is preferably 50°C to 120°C, more preferably 50°C to 105°C, and even more preferably 60°C to 105°C. Furthermore, the treatment time can be appropriately set depending on the desired performance and is not particularly limited, but is preferably 30 seconds to 30 minutes, more preferably 30 seconds to 15 minutes, and even more preferably 1 minute to 10 minutes.

[0091] The present invention will be described in more detail below with reference to examples that clearly demonstrate the effects of the present invention, but the present invention is not limited to the following examples.

[0092] [Digital Bioassay] Two holes were drilled in a 5 mm thick piece of glass cut into a 25 mm square, and one side was hydrophobically coated with CYTOP CTL-816AP (manufactured by AGC). Kapton (registered trademark) double-sided tape cut into the shape of a flow channel was attached to this glass piece, and the fine well films for bioassay obtained in the Examples and Comparative Examples were further attached to prepare flow cells.

[0093] Next, 10 mM (the concentration is the final concentration after mixing; the same applies below) of 4-methylumbelliferyl phosphate (4MUP), a 4-MU-generating substrate that generates 4-methylumbelliferone (4-MU, excitation wavelength 365 nm, fluorescence wavelength 445 nm) through an enzymatic reaction (dephosphorylation reaction), was mixed with 0.1% of the nonionic surfactant TWEEN (registered trademark) 20 (Merck P7949), and alkaline phosphatase (ALP), a dephosphorylating enzyme, to prepare an ALP aqueous solution (pH = 9.25) containing 1 M diethanolamine and 1 mM magnesium chloride. The concentration of the ALP aqueous solution was 1 pM.

[0094] The ALP aqueous solution was then poured into the fabricated flow cell through a hole drilled in the glass, and then perfluorocarbon oil was poured into the flow cell as an encapsulating oil to remove excess ALP aqueous solution, and the ALP aqueous solution was encapsulated in the chamber on the film. Subsequently, the volatile perfluorocarbon oil was replaced with nonvolatile perfluoropolyether oil to prevent the encapsulating oil from being lost due to volatilization, which would expose the chamber to the air phase and cause the ALP aqueous solution to evaporate.

[0095] Fluorescence image observation was then performed using the following equipment configuration. Images were taken 10 minutes after the perfluorocarbon oil was poured in. Microscope: IX83 (Olympus Corporation) Camera: Neo sCMOS camera (Andor Corporation) Objective lens magnification: 20x Light source: X-Cite (registered trademark) XYLIS LED light source for fluorescence microscopes (Excelitas Technologies Corporation) Filter unit: FF01-377 / 50 excitation filter (Semrock Corporation, transmits 352-402 nm) FF409-Di03 dichroic mirror (Semrock Corporation, transmits 409 nm or higher) FF02-447 / 60 emission filter (Semrock Corporation, transmits 417-477 nm)

[0096] Here, the sample was excited with excitation light reflected by the FF409-Di03 filter unit and transmitted through the FF01-377 / 50 excitation filter. The emitted fluorescence was then transmitted through the FF409-Di03 filter unit and the FF02-447 / 60 emission filter to acquire fluorescence images. The chamber containing the fluorescent molecule 4-MU exhibited a brighter fluorescence intensity than the surrounding area, and was therefore referred to as a bright spot. Image analysis was performed using ImageJ / Fiji. The size of the bright spot was approximately 5-6 pixels in diameter on the image. Therefore, when a circle with a radius of 3 pixels was drawn around the center of the bright spot, the average value of the pixel values ​​within the circle was defined as the fluorescence intensity (IF) of the bright spot. The region within a circle with a radius of 5 pixels but not within a radius of 3 pixels was defined as the background region of the bright spot. The mean value (IB) and standard deviation (SDB) of the pixels in the background region were calculated, and the S / N ratio was calculated using the following formula. Note that any other bright spots within the background region were excluded from this analysis. S / N ratio = (IF-IB) / SDB

[0097] Example 1 First, trimethylolpropane triacrylate (M350 manufactured by Toagosei Co., Ltd.), N-vinylpyrrolidone, Omnirad 184 (manufactured by IGM Resins B.V.), and 2-(diethylamino)ethyl methacrylate as a fluorescence regulator were mixed in a ratio of 67:33:5.5:5 by mass to prepare a photosensitive resin composition of Example 1.

[0098] Next, a nickel plate-like mold (well density 12 million / cm) was used, in which cylindrical protrusions with a diameter of 2 μm and a height of 2 μm were arranged on three sides at a pitch of 3 μm. 2 The above materials were subjected to a release treatment using OPTOOL HD-2100TH manufactured by Daikin Industries, Ltd.

[0099] Next, a cyclic olefin resin film (ZeonorFilm (registered trademark) manufactured by Nippon Zeon Co., Ltd., thickness 188 μm) that had been subjected to a surface corona treatment in advance was used as a substrate, and the photosensitive resin composition of Example 1 was dropped onto this substrate and sandwiched between the fine uneven structure surfaces of a flat plate-like mold, while simultaneously being stretched using a hand roller. After curing by UV exposure from the resin film side to form a resin layer, the laminate of the resin film and resin layer was peeled off from the flat plate-like mold, and a fine well film for bioassay in which the resin film and resin layer were integrated was obtained. The surface of the obtained fine well film for bioassay of Example 1 was covered with fine wells (well density 12 million / cm) in which cylindrical wells with a diameter of 2 μm and a depth of 2 μm were arranged on three sides at a pitch of 3 μm. 2 The fine well film was observed using a scanning electron microscope (hereinafter referred to as SEM). The equipment and microscopic conditions used are as follows: Equipment: HITACHI s-5500 Acceleration voltage: 10 kV Mode: Normal Observation surface treatment: Os coating

[0100] A digital bioassay using an ALP solution was performed using the obtained bioassay microwell film of Example 1. As a result, bright spots were detected, and the S / N ratio was 42, indicating that digital bioassay was possible. In addition, the adhesion between the resin layer having a microrelief structure of microwells on its surface and the substrate was good.

[0101] The pattern shape of the obtained fine well film for bioassay of Example 1 was observed with a metallurgical microscope and evaluated according to the following criteria: ◯: 3 μm hole pattern was formed neatly; Δ: hole pattern was obtained, but the pattern edges were jagged; ×: 3 μm hole pattern was not formed.

[0102] Example 2 A photosensitive resin composition of Example 2 was prepared by mixing trimethylolpropane triacrylate (M350 manufactured by Toagosei Co., Ltd.), N-vinylpyrrolidone, Omnirad 184 (manufactured by IGM Resins B.V.), and 2-(diethylamino)ethyl methacrylate as a fluorescence regulator in a ratio of 67:33:5.5:3 by mass. The photosensitive resin composition of Example 2 was prepared in the same manner as in Example 1, except that the photosensitive resin composition of Example 2 was used instead of the photosensitive resin composition of Example 1. Microwells (well density: 12 million / cm) were fabricated in which cylindrical wells with a diameter of 2 μm and a depth of 2 μm were arranged on three sides at a pitch of 3 μm. 2 A fine well film for bioassay of Example 2 was obtained, on the surface of which the above-mentioned films were formed.

[0103] A digital bioassay using an ALP solution was performed using the obtained fine well film for bioassay of Example 2. As a result, bright spots were detected, and the S / N ratio was 36, making digital bioassay possible. Furthermore, the adhesion between the resin layer having a fine uneven structure of fine wells on its surface and the substrate was good. The pattern shape of the obtained fine well film for bioassay of Example 2 was observed with a metallurgical microscope and evaluated using the same evaluation criteria as in Example 1.

[0104] Example 3 A photosensitive resin composition of Example 3 was prepared by mixing trimethylolpropane triacrylate (M350 manufactured by Toagosei Co., Ltd.), N-vinylpyrrolidone, Omnirad 184 (manufactured by IGM Resins B.V.), and 2-(diethylamino)ethyl methacrylate as a fluorescence regulator in a ratio of 67:33:5.5:1 by mass. The photosensitive resin composition of Example 3 was prepared in the same manner as in Example 1, except that the photosensitive resin composition of Example 3 was used instead of the photosensitive resin composition of Example 1. Microwells (well density: 12 million / cm) were fabricated in which cylindrical wells with a diameter of 2 μm and a depth of 2 μm were arranged on three sides at a pitch of 3 μm. 2 A fine well film for bioassay of Example 3 was obtained, on the surface of which the above-mentioned films were formed.

[0105] A digital bioassay using an ALP solution was performed using the obtained fine well film for bioassay of Example 3. As a result, bright spots were detected, and the S / N ratio was 44, making digital bioassay possible. In addition, the adhesion between the resin layer having a fine uneven structure of fine wells on the surface and the substrate was good. In addition, the pattern shape of the obtained fine well film for bioassay of Example 3 was observed with a metallurgical microscope and evaluated using the same evaluation criteria as in Example 1.

[0106] Example 4 Bisphenol A EO-modified (n≈2) diacrylate (M211B manufactured by Toagosei Co., Ltd.), N-vinylpyrrolidone, Omnirad 184 (manufactured by IGM Resins B.V.), and 2-(diethylamino)ethyl methacrylate as a fluorescence regulator were mixed in a ratio of 58:33:5.5:10 parts by mass to prepare the photosensitive resin composition of Example 4. Fine wells (well density 12 million / cm) in which cylindrical wells with a diameter of 2 μm and a depth of 2 μm were arranged on three sides at a pitch of 3 μm were fabricated in the same manner as in Example 1, except that the photosensitive resin composition of Example 4 was used instead of the photosensitive resin composition of Example 1. 2 A fine well film for bioassay of Example 4 was obtained, on the surface of which the above-mentioned films were formed.

[0107] A digital bioassay using an ALP solution was performed using the obtained fine well film for bioassay of Example 4. As a result, bright spots were detected, and the S / N ratio was 44, making digital bioassay possible. Furthermore, the adhesion between the resin layer having a fine uneven structure of fine wells on its surface and the substrate was good. The pattern shape of the obtained fine well film for bioassay of Example 4 was observed with a metallurgical microscope and evaluated using the same evaluation criteria as in Example 1.

[0108] Example 5 A photosensitive resin composition of Example 5 was prepared by mixing trimethylolpropane triacrylate (M350 manufactured by Toagosei Co., Ltd.), N-vinylpyrrolidone, Omnirad 184 (manufactured by IGM Resins B.V.), and 2-(diethylamino)ethyl methacrylate as a fluorescence regulator in a ratio of 36:33:5.5:36 parts by mass. A photosensitive resin composition of Example 5 was prepared in the same manner as in Example 1, except that the photosensitive resin composition of Example 5 was used instead of the photosensitive resin composition of Example 1. Microwells (well density: 12 million / cm) were fabricated in which cylindrical wells with a diameter of 2 μm and a depth of 2 μm were arranged on three sides at a pitch of 3 μm. 2 A fine well film for bioassay of Example 4 was obtained, on the surface of which the above-mentioned films were formed.

[0109] A digital bioassay using an ALP solution was performed using the obtained fine well film for bioassay of Example 5. As a result, bright spots were detected, and the S / N ratio was 46, making digital bioassay possible. In addition, the adhesion between the resin layer having a fine uneven structure of fine wells on the surface and the substrate was good. In addition, the pattern shape of the obtained fine well film for bioassay of Example 5 was observed with a metallurgical microscope and evaluated using the same evaluation criteria as in Example 1.

[0110] Comparative Example 1 Trimethylolpropane triacrylate (M350 manufactured by Toagosei Co., Ltd.), a urethane oligomer (CN991 manufactured by Sartomer Corporation) which is a photopolymerizable oligomer, N-vinylpyrrolidone, and Omnirad 184 (manufactured by IGM Resins B.V.) were mixed in a ratio of 57:33:10:5.5 parts by mass to prepare a photosensitive resin composition of Comparative Example 1. A photosensitive resin composition of Comparative Example 1 was prepared in the same manner as in Example 1, except that the photosensitive resin composition of Comparative Example 1 was used instead of the photosensitive resin composition of Example 1. Microwells (well density 12 million / cm) were prepared in which cylindrical wells with a diameter of 2 μm and a depth of 2 μm were arranged on three sides at a pitch of 3 μm. 2 A fine well film of Comparative Example 1 was obtained, on the surface of which were formed the above-mentioned films.

[0111] A digital bioassay using an ALP solution was performed using the fine well film obtained in Comparative Example 1. As a result, no bright spots were detected by the digital bioassay, and the result was unsuitable. The pattern shape of the fine well film for bioassay obtained in Comparative Example 1 was observed with a metallurgical microscope and evaluated using the same evaluation criteria as in Example 1.

[0112] Comparative Example 2 Trimethylolpropane triacrylate (M350 manufactured by Toagosei Co., Ltd.), N-vinylpyrrolidone, and Omnirad 184 (manufactured by IGM Resins B.V.) were mixed in a ratio of 67:33:5.5 parts by mass to prepare a photosensitive resin composition of Comparative Example 2. Fine wells (well density 12 million / cm) in which cylindrical wells with a diameter of 2 μm and a depth of 2 μm were arranged on three sides at a pitch of 3 μm were prepared in the same manner as in Example 1, except that the photosensitive resin composition of Comparative Example 2 was used instead of the photosensitive resin composition of Example 1. 2 A fine well film of Comparative Example 2 was obtained, on the surface of which were formed the above-mentioned films.

[0113] A digital bioassay using an ALP solution was performed using the fine well film obtained in Comparative Example 2. As a result, no bright spots were detected by the digital bioassay, and the result was unsuitable. In addition, the pattern shape of the fine well film for bioassay obtained in Comparative Example 2 was observed with a metallurgical microscope and evaluated using the same evaluation criteria as in Example 1.

[0114] Comparative Example 3 Trimethylolpropane triacrylate (M350 manufactured by Toagosei Co., Ltd.), N-vinylpyrrolidone, Omnirad 184 (manufactured by IGM Resins B.V.), and 2-acryloyloxyethyl acidic phosphate (Light Acrylate P-1A(N), manufactured by Kyoeisha Chemical Co., Ltd.) were mixed in a ratio of 67:33:5.5:5 by mass to prepare a photosensitive resin composition of Comparative Example 3. A photosensitive resin composition of Comparative Example 3 was prepared in the same manner as in Example 1, except that the photosensitive resin composition of Comparative Example 3 was used instead of the photosensitive resin composition of Example 1. A photosensitive resin composition of Comparative Example 3 was prepared in the same manner as in Example 1, in which cylindrical wells with a diameter of 2 μm and a depth of 2 μm were arranged on three sides at a pitch of 3 μm (well density: 12 million / cm). 2 A fine well film of Comparative Example 3 was obtained, on the surface of which were formed the above-mentioned films.

[0115] A digital bioassay using an ALP solution was performed using the fine well film obtained in Comparative Example 3. As a result, no bright spots were detected by the digital bioassay, and the result was unsuitable. In addition, the pattern shape of the fine well film for bioassay obtained in Comparative Example 3 was observed with a metallurgical microscope and evaluated using the same evaluation criteria as in Example 1.

[0116] Comparative Example 4 Trimethylolpropane triacrylate (M350 manufactured by Toagosei Co., Ltd.), N-vinylpyrrolidone, Omnirad 184 (manufactured by IGM Resins B.V.), and 2-acryloyloxyethyl acidic phosphate (Light Acrylate P-1A(N), manufactured by Kyoeisha Chemical Co., Ltd.) were mixed in a ratio of 67:33:5.5:0.5 parts by mass to prepare a photosensitive resin composition of Comparative Example 4. A photosensitive resin composition of Comparative Example 4 was prepared in the same manner as in Example 1, except that the photosensitive resin composition of Comparative Example 4 was used instead of the photosensitive resin composition of Example 1. A photosensitive resin composition of Comparative Example 4 was prepared in the same manner as in Example 1, in which cylindrical wells with a diameter of 2 μm and a depth of 2 μm were arranged on three sides at a pitch of 3 μm (well density: 12 million / cm). 2 A fine well film of Comparative Example 4 was obtained, on the surface of which were formed the above-mentioned films.

[0117] A digital bioassay using an ALP solution was performed using the obtained fine well film of Comparative Example 4. Bright spots with an S / N ratio of 30 were detected, but the brightness was insufficient for a digital bioassay. Furthermore, the adhesion between the resin layer having a fine uneven structure of fine wells on its surface and the substrate was good. The pattern shape of the obtained fine well film for bioassay of Comparative Example 4 was observed with a metallurgical microscope and evaluated using the same evaluation criteria as in Example 1.

[0118] Comparative Example 5 Trimethylolpropane triacrylate (M350 manufactured by Toagosei Co., Ltd.), N-vinylpyrrolidone, Omnirad 184 (manufactured by IGM Resins B.V.), and 2-acryloyloxyethyl acidic phosphate (Light Acrylate P-1A(N), manufactured by Kyoeisha Chemical Co., Ltd.) were mixed in a ratio of 25:33:5.5:42 parts by mass to prepare a photosensitive resin composition of Comparative Example 5. A photosensitive resin composition of Comparative Example 5 was prepared in the same manner as in Example 1, except that the photosensitive resin composition of Comparative Example 5 was used instead of the photosensitive resin composition of Example 1. A photosensitive resin composition of Comparative Example 5 was prepared in the same manner as in Example 1, in which cylindrical wells with a diameter of 2 μm and a depth of 2 μm were arranged on three sides at a pitch of 3 μm (well density: 12 million / cm). 2 A fine well film of Comparative Example 5 was obtained, on the surface of which were formed the above-mentioned films.

[0119] When the obtained fine well film of Comparative Example 5 was observed by SEM, a hole pattern was obtained, but the pattern edge portion was jagged, and it was unsuitable as a fine well film for bioassay. In addition, the pattern shape of the obtained fine well film for bioassay of Comparative Example 5 was observed with a metallurgical microscope and evaluated according to the same evaluation criteria as in Example 1.

[0120] Table 1 shows the materials and effects of Examples 1 to 5 and Comparative Examples 1 to 5.

[0121] As shown in Table 1, in Examples 1 to 5, in which the resin layer contained a modified (meth)acrylate resin having an amino group, fluorescence derived from the 4-MU dye at a wavelength of around 450 nm was obtained with a good S / N ratio, and fluorescence observation in the visible light region was possible even when using a 4-MU-generating substrate, etc., confirming the realization of a fine well film for bioassay with a high S / N ratio and improved quantitativeness. It was also confirmed that the modified (meth)acrylate resin having an amino group has a fluorescence-adjusting function.

[0122] Furthermore, in all of Examples 1 to 5, a modified (meth)acrylate having an amino group was added to the photosensitive resin composition. This confirmed that the modified (meth)acrylate having an amino group functions as a fluorescence regulator, and that this fluorescence regulator can increase the sensitivity of the bioassay. Furthermore, while an S / N ratio of 3 times or more, preferably 10 times or more, is required for the industrialization of digital bioassays, the bioassay microwell film of the present invention achieved an S / N ratio well above 30 times, demonstrating particularly excellent quantitative performance.

[0123] Furthermore, a comparison of Examples 1 to 5 confirmed that the S / N ratio of the digital bioassay can be adjusted by adjusting the blending ratio of the fluorescence adjuster.

[0124] The present invention is not limited to the above-described embodiment, and various modifications can be made to the embodiment. In the above-described embodiment, the size, shape, etc. shown in the drawings are not limited to these, and can be appropriately modified within the scope of the present invention.

[0125] The bioassay microwell film etc. of the present invention has a fluorescence adjustment function, and allows fluorescence observation in the visible light region even when using, for example, a 4-MU generating substrate, and has a high S / N ratio and improved quantitativeness, so it can be widely and effectively used in digital bioassays, single-molecule enzyme assays, etc. In particular, the bioassay microwell film etc. of the present invention can be applied to industrial practical uses as a novel material that achieves higher sensitivity than conventional materials even when the microwells are densely packed.

[0126] DESCRIPTION OF SYMBOLS 1 Bioassay fine well film 11 Substrate 12 Resin layer 13 Recess F One surface Z Z-axis direction

Claims

1. A fine well film for bioassays comprising at least a substrate and a resin layer provided on one side of the substrate and having fine wells on its surface, the resin layer containing a modified (meth)acrylate resin having an amino group, and the molar ratio of the amino group to the (meth)acrylate unit in the modified (meth)acrylate resin is 0.010 to 0.

500.

2. The fine well film for bioassay according to claim 1, wherein the resin layer is a cured product of a photosensitive resin composition containing at least a multifunctional (meth)acrylate, an amino group-containing (meth)acrylic acid alkyl ester, and a photopolymerization initiator.

3. The fine well film for bioassay according to claim 2, wherein the photosensitive resin composition further contains a nitrogen-containing vinyl monomer.

4. The fine well film for bioassay according to claim 1, wherein the amino group includes an N-alkylamino group and / or an N,N-dialkylamino group.

5. The fine well film for bioassay according to claim 1, wherein the amino group comprises one selected from the group consisting of an N-methylamino group, an N-ethylamino group, an N,N-dimethylamino group, an N-methyl-N-ethylamino group, and an N,N-diethylamino group.

6. The fine well film for bioassay according to claim 1, wherein the substrate is a cyclic olefin resin film.

7. The well density of the fine wells is 1 million / cm 2 The fine well film for bioassay according to claim 1 .

8. The fine well film for bioassay according to claim 1, which is for use in a single molecule enzyme assay method.

9. A photosensitive resin composition for forming a fine well film for bioassay, comprising at least (A) a polyfunctional (meth)acrylate, (B) an alkyl (meth)acrylate ester, and (C) a photopolymerization initiator, wherein the alkyl (meth)acrylate ester (B) comprises an alkyl (meth)acrylate ester having an amino group, and the molar ratio of the amino group to the (meth)acrylate units contained in the photosensitive resin composition is 0.010 to 0.

500.

10. The photosensitive resin composition for forming a fine well film for bioassay according to claim 9, wherein the content of said (A) polyfunctional (meth)acrylate is 50.0 to 90.0 mass% relative to the total amount of said photosensitive resin composition, the content of said (B) amino group-containing (meth)acrylic acid alkyl ester is 0.1 to 10.0 mass% relative to the total amount of said photosensitive resin composition, and the content of said (C) photopolymerization initiator is 0.5 to 10.0 mass% relative to the total amount of said photosensitive resin composition.

11. The photosensitive resin composition for forming a fine well film for bioassay according to claim 9, further comprising (D) a nitrogen-containing vinyl monomer.

12. The photosensitive resin composition for forming a fine well film for bioassay according to claim 11, wherein the content of the nitrogen-containing vinyl monomer (D) is 10.0 to 50.0 mass % relative to the total amount of the photosensitive resin composition.

13. A method for producing a fine well film for bioassays as described in claim 1, comprising the steps of: applying the photosensitive resin composition for forming a fine well film for bioassays as described in claim 9 onto a substrate or a mold; pressing the photosensitive resin composition between the substrate and the mold; curing the photosensitive resin composition by exposure to light to obtain a cured product; and peeling off the cured product from the mold.

14. The method for producing a fine well film for bioassays according to claim 13, wherein the coating step includes coating the photosensitive resin composition onto at least the substrate, and further includes a penetration step of permeating the photosensitive resin composition into the substrate prior to the pressing step.

Citation Information

Patent Citations

  • Micro-chamber used for detecting unimolecular enzyme activity

    JP2004309405A

  • Microwell film for bioassay, photosensitive resin composition for forming microwell film for bioassay, and method for manufacturing microwell film for bioassay

    WO2021002388A1