Secondary battery
The secondary battery incorporates a lithium composite oxide with a specific nickel content and a lithium fluoroborate covering layer, analyzed using TOF-SIMS, to enhance battery performance by preventing electrical resistance increase and maintaining high capacity, addressing the insufficiencies in existing secondary battery configurations.
Patent Information
- Application Number
- PCT/JP2024/012482
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-03
AI Technical Summary
Secondary batteries exhibit insufficient battery characteristics despite various studies, necessitating the development of a configuration that enhances their performance.
A secondary battery with a positive electrode active material layer comprising lithium composite oxide with a layered rock salt crystal structure, containing 80-100 mole percent nickel and other elements, and a covering portion of lithium fluoroborate, analyzed using time-of-flight secondary ion mass spectrometry to optimize ion intensity profiles, which prevents the increase in electrical resistance and maintains high battery capacity.
The battery achieves excellent battery characteristics by electrochemically protecting the surface, suppressing charge transfer inhibition and oxidative decomposition, thereby maintaining high capacity even after repeated charging and discharging.
Smart Images

Figure JP2024012482_03102024_PF_FP_ABST
Abstract
Description
secondary battery
[0001] The present technology relates to a secondary battery.
[0002] Due to the widespread use of various electronic devices such as mobile phones, secondary batteries have been developed as small, lightweight power sources that can provide high energy density. These secondary batteries contain a positive electrode, a negative electrode, and an electrolyte solution, and various studies have been conducted on the configuration of these secondary batteries.
[0003] Specifically, the assembled battery is charged and discharged under heating, and the electrolyte (LiPF 6 and LiBF 4 ) is present on the surface of the positive electrode, and the coating components are analyzed using time-of-flight secondary ion mass spectrometry (TOF-SIMS) (see, for example, Patent Document 1).
[0004] JP 2013-062026 A
[0005] Although various studies have been conducted on the configuration of secondary batteries, the battery characteristics of the secondary batteries are still insufficient and there is room for improvement.
[0006] There is a demand for a secondary battery that can provide excellent battery characteristics.
[0007] A secondary battery according to one embodiment of the present technology includes a positive electrode including a positive electrode active material layer, a negative electrode, and an electrolyte. The positive electrode active material layer includes a plurality of positive electrode active material particles, each of which includes a core including a lithium composite oxide and a coating portion provided on the surface of the core. The lithium composite oxide has a layered rock salt crystal structure and includes lithium, nickel, and other elements as constituent elements. When the sum of the nickel content in the lithium composite oxide and the content of the other elements in the lithium composite oxide is taken as 100 molar parts, the nickel content is 80 molar parts to 100 molar parts. Depth analysis of the positive electrode active material layer using time-of-flight secondary ion mass spectrometry revealed that NiO2 - and a first negative secondary ion derived from LiBO 2 F - and second negative secondary ions derived from the first negative secondary ions are detected, and a first depth profile representing a change in the ionic intensity of the first negative secondary ions in the depth direction and a second depth profile representing a change in the ionic intensity of the second negative secondary ions in the depth direction are obtained. In the first depth profile, the ionic intensity of the first negative secondary ions increases in the depth direction, and in the second depth profile, the ionic intensity of the second negative secondary ions decreases in the depth direction, and the second depth profile has a step region where the ionic intensity of the second negative secondary ions temporarily stops decreasing in the depth direction while the ionic intensity of the first negative secondary ions increases in the depth direction.
[0008] According to a secondary battery of one embodiment of the present technology, the positive electrode active material layer includes a plurality of positive electrode active material particles, each of the positive electrode active material particles includes a core (lithium composite oxide) and a coating portion, the lithium composite oxide has a layered rock salt type crystal structure and includes lithium, nickel, and other elements as constituent elements, the content of nickel in the lithium composite oxide is 80 parts by mole or more and 100 parts by mole or less, and a depth direction analysis of the positive electrode active material layer using time-of-flight secondary ion mass spectrometry detects first negative secondary ions (NiO - ) and a second negative secondary ion (LiBO). 2 F - ) is obtained, and in the first depth profile, the ionic strength of the first negative secondary ions increases in the depth direction, and in the second depth profile, the ionic strength of the second negative secondary ions decreases in the depth direction. The second depth profile has a step region where the ionic strength of the second negative secondary ions temporarily stops decreasing in the depth direction while the ionic strength of the first negative secondary ions increases in the depth direction, thereby obtaining excellent battery characteristics.
[0009] Note that the effects of the present technology are not necessarily limited to the effects described here, but may be any of a series of effects related to the present technology described below.
[0010] Fig. 1 is a perspective view showing the configuration of a secondary battery according to an embodiment of the present technology. Fig. 2 is a cross-sectional view showing the configuration of the battery element shown in Fig. 1. Fig. 3 is a cross-sectional view showing the configuration of a positive electrode active material particle. Fig. 4 is a diagram showing the results of analysis of a positive electrode active material layer in the depth direction using time-of-flight secondary ion mass spectrometry. Fig. 5 is a block diagram showing the configuration of an application example of a secondary battery. Fig. 6 is a cross-sectional view showing the configuration of a test secondary battery.
[0011] Hereinafter, an embodiment of the present technology will be described in detail with reference to the drawings. The description will be made in the following order: 1. Secondary battery 1-1. Configuration 1-2. Physical properties 1-3. Operation 1-4. Manufacturing method 1-5. Actions and effects 2. Modifications 3. Uses of secondary battery
[0012] 1. Secondary Battery First, a secondary battery according to an embodiment of the present technology will be described.
[0013] The secondary battery described here is a secondary battery that obtains battery capacity by utilizing the absorption and desorption of electrode reactants, and is equipped with a positive electrode, a negative electrode, and an electrolyte.
[0014] The charge capacity of the negative electrode is preferably larger than the discharge capacity of the positive electrode. That is, the electrochemical capacity per unit area of the negative electrode is preferably larger than the electrochemical capacity per unit area of the positive electrode. This is to prevent deposition of electrode reactants on the surface of the negative electrode during charging.
[0015] The type of electrode reactant is not particularly limited, but specifically includes light metals such as alkali metals and alkaline earth metals. Specific examples of alkali metals include lithium, sodium, and potassium, and specific examples of alkaline earth metals include beryllium, magnesium, and calcium.
[0016] In the following, we will take the case where the electrode reactant is lithium as an example. A secondary battery that obtains battery capacity by utilizing the absorption and desorption of lithium is called a lithium ion secondary battery. In this lithium ion secondary battery, lithium is absorbed and desorbed in the ionic state.
[0017] <1-1. Configuration> Fig. 1 shows a perspective configuration of a secondary battery. Fig. 2 shows a cross-sectional configuration of a battery element 20 shown in Fig. 1. Fig. 3 shows a cross-sectional configuration of a positive electrode active material particle 210.
[0018] 1 shows a state in which the exterior film 10 and the battery element 20 are separated from each other, and a cross section of the battery element 20 taken along the XZ plane is shown by a broken line. In FIG. 2, only a part of the battery element 20 is shown.
[0019] As shown in FIGS. 1 and 2, this secondary battery includes an exterior film 10, a battery element 20, a positive electrode lead 31, a negative electrode lead 32, and sealing films 41 and .
[0020] As described above, the secondary battery described here uses flexible or pliable exterior film 10 as an exterior member for housing battery element 20. Therefore, the secondary battery shown in Fig. 1 is a so-called laminate film type secondary battery.
[0021] 1, the exterior film 10 has a bag-like structure that is sealed with the battery element 20 housed therein. As a result, the exterior film 10 houses a positive electrode 21, a negative electrode 22, and a separator 23, which will be described later.
[0022] Here, the exterior film 10 is a single film-like member that is folded in a folding direction F. The exterior film 10 is provided with a recessed portion 10U (a so-called deep drawn portion) for accommodating the battery element 20.
[0023] Specifically, the exterior film 10 is a three-layer laminate film in which a fusion layer, a metal layer, and a surface protection layer are laminated in this order from the inside out, and when the exterior film 10 is folded, the outer peripheral edges of the opposing fusion layers are fused to each other. The fusion layer contains a polymer compound such as polypropylene. The metal layer contains a metal material such as aluminum. The surface protection layer contains a polymer compound such as nylon.
[0024] However, the configuration (number of layers) of the exterior film 10 is not particularly limited, and may be one layer, two layers, or four or more layers.
[0025] [Battery Element] The battery element 20 is housed inside the exterior film 10. The battery element 20 is a so-called power generating element, and includes a positive electrode 21, a negative electrode 22, and a separator 23, as shown in Figures 1 and 2 .
[0026] Here, battery element 20 is a so-called wound electrode body, and therefore positive electrode 21 and negative electrode 22 are wound around winding axis P while facing each other via separator 23. Winding axis P is a virtual axis extending in the Y-axis direction.
[0027] There are no particular limitations on the three-dimensional shape of battery element 20. Here, battery element 20 has a flat three-dimensional shape, and therefore the shape of a cross section (cross section along the XZ plane) of battery element 20 intersecting winding axis P is a flat shape defined by major axis J1 and minor axis J2.
[0028] The major axis J1 is an imaginary axis extending in the X-axis direction and has a length greater than that of the minor axis J2. The minor axis J2 is an imaginary axis extending in the Z-axis direction intersecting the X-axis direction and has a length less than that of the major axis J1. Here, the three-dimensional shape of the battery element 20 is a flattened cylinder, and therefore the cross-sectional shape of the battery element 20 is a flattened, approximately elliptical shape.
[0029] (Positive Electrode) As shown in FIG. 2, the positive electrode 21 includes a positive electrode current collector 21A and a positive electrode active material layer 21B.
[0030] The positive electrode current collector 21A has a pair of surfaces on which the positive electrode active material layer 21B is provided. The positive electrode current collector 21A contains a conductive material such as a metal material, and a specific example of the conductive material is aluminum.
[0031] The positive electrode active material layer 21B contains one or more types of positive electrode active materials that absorb and release lithium. However, the positive electrode active material layer 21B may further contain one or more types of other materials such as a positive electrode binder and a positive electrode conductive agent. The method for forming the positive electrode active material layer 21B is not particularly limited, but specifically includes a coating method.
[0032] Here, the positive electrode active material layer 21B is provided on both sides of the positive electrode current collector 21A. However, the positive electrode active material layer 21B may be provided on only one side of the positive electrode current collector 21A, on the side where the positive electrode 21 faces the negative electrode 22.
[0033] Specifically, as shown in Fig. 3, the positive electrode active material layer 21B includes a plurality of particulate positive electrode active material particles (hereinafter referred to as "a plurality of positive electrode active material particles 210"). The positive electrode active material particles 210 include a central portion 210X and a coating portion 210Y.
[0034] The central portion 210X contains one or more types of lithium composite oxides that absorb and release lithium. The lithium composite oxides have a layered rock-salt crystal structure and contain lithium, nickel, and other elements as constituent elements. The other elements are one or more types of elements other than lithium and nickel.
[0035] However, the lithium composite oxide is designed to have a sufficiently large nickel content. Specifically, when the sum of the nickel content in the lithium composite oxide and the contents of other elements in the lithium composite oxide is taken as 100 parts by mol, the nickel content is 80 to 100 parts by mol. As is clear from the fact that the upper limit of the nickel content is 100 parts by mol, the lithium composite oxide may or may not contain other elements as constituent elements.
[0036] In addition, when the lithium composite oxide contains two or more types of other elements as constituent elements, the content of the other elements in the lithium composite oxide described above is the sum of the respective contents of the two or more types of other elements contained as constituent elements in the lithium composite oxide.
[0037] That is, when the content of nickel in the lithium composite oxide is C1 (mol) and the content of other elements in the lithium composite oxide is C2 (mol), the nickel content C calculated by the formula C = [C1 / (C1 + C2)] × 100 is 80 mol % to 100 mol %.
[0038] The reason why the content ratio C is 80 mol % to 100 mol % is that the potential for absorbing and releasing lithium is lowered compared to when the content ratio C is less than 80 mol %, and therefore a high battery capacity can be obtained.
[0039] The type of other element is not particularly limited, but specific examples include cobalt, aluminum, manganese, zirconium, titanium, molybdenum, tantalum, chromium, niobium, iron, copper, zinc, vanadium, magnesium, tungsten, sulfur, strontium, boron, sodium, and fluorine, because sufficient battery capacity can be obtained.
[0040] More specifically, the lithium composite oxide contains one or more of the compounds represented by formula (1). The compound represented by formula (1) contains another element E as a constituent element.
[0041] Li a Ni b E 1-b O 2 ... (1) (E is at least one of Co, Al, Mn, Zr, Ti, Mo, Ta, Cr, Nb, Fe, Cu, Zn, V, Mg, W, S, Sr, B, Na, and F. a and b satisfy 0.8≦a≦1.05 and 0.8≦b≦1.0, respectively.)
[0042] The positive electrode active material layer 21B may further contain one or more other positive electrode active materials that absorb and release lithium. The other positive electrode active materials include a lithium-containing compound, and the lithium composite oxide described above is excluded from the lithium-containing compound described here.
[0043] The lithium-containing compound is a compound containing lithium and one or more transition metal elements as constituent elements, and may further contain one or more additional elements as constituent elements. The type of additional element (excluding lithium and transition metal elements) is not particularly limited, but specifically, it is an element belonging to Groups 2 to 15 of the long period periodic table. The type of lithium-containing compound is not particularly limited, but specifically, it is an oxide, a phosphate compound, a silicate compound, a borate compound, etc.
[0044] A specific example of the oxide is LiNiO 2 , LiCoO 2 , LiCo 0.98 Al 0.01 Mg 0.01 O 2 , LiNi 0.5 Co 0.2 Mn 0.3 O 2 and LiMn 2 O 4 Specific examples of phosphate compounds include LiFePO 4 , LiMnPO 4 and LiFe 0.5 Mn 0.5 P.O. 4 And so on.
[0045] The covering portion 210Y is provided on the surface of the central portion 210X, and therefore covers the surface of the central portion 210X.
[0046] Here, the covering portion 210Y covers the entire surface of the central portion 210X. However, the covering portion 210Y may cover only a portion of the surface of the central portion 210X. In this case, a plurality of covering portions 210Y separated from one another may cover the surface of the central portion 210X.
[0047] The covering portion 210Y is made of LiBO (LiFePO4) 2 F - The composition of the material forming the covering portion 210Y is not particularly limited as long as the covering portion 210Y is formed using the second negative secondary ions.
[0048] The coating portion 210Y is provided on the surface of the central portion 210X, and the coating portion 210Y contains a material formed using second negative secondary ions because an increase in the electrical resistance of the positive electrode 21 is suppressed even if a lithium composite oxide (content ratio C≧80 mol%) is used as the material for forming the central portion 210X.
[0049] In particular, as described above, by using a lithium composite oxide (content ratio C≧80 mol %) as the material for forming the central portion 210X, a high battery capacity can be obtained.
[0050] However, when a lithium composite oxide (content ratio C≧80 mol%) is used, the surface activity of the positive electrode 21 increases during charging, making the electrolyte more susceptible to oxidative decomposition on the surface of the positive electrode 21. When the electrolyte is oxidatively decomposed, decomposition products that become resistance components are more likely to be formed, and these decomposition products are more likely to accumulate on the surface of the central portion 210X. Therefore, the charge transfer reaction is more likely to be inhibited in the central portion 210X, making the electrical resistance of the positive electrode 21 more likely to increase. As a result, the battery capacity is more likely to decrease with repeated charging and discharging.
[0051] However, when the coating portion 210Y is provided on the surface of the central portion 210X and the three physical property conditions described below regarding the physical properties of the positive electrode active material layer 21B are satisfied, the surface of the central portion 210X is electrochemically protected by the coating portion 210Y. This coating portion 210Y has high oxidation resistance and is ionic conductive but not electronic conductive. As a result, the coating portion 210Y suppresses the formation of decomposition products and suppresses their accumulation on the surface of the central portion 210X, thereby suppressing the charge transfer reaction from being inhibited and also suppressing the oxidative decomposition of the electrolyte on the surface of the central portion 210X. Therefore, the electrical resistance of the positive electrode 21 is less likely to increase, and the battery capacity is less likely to decrease even with repeated charging and discharging.
[0052] As described above, the covering portion 210Y contains a material formed using the second negative secondary ions, and therefore preferably contains lithium, boron, and fluorine as constituent elements, because the surface of the central portion 210X is more likely to be electrochemically protected by the covering portion 210Y.
[0053] Among these, the covering portion 210Y is made of lithium fluoroborate (LiBOF 2 It is more preferable that the core 210X contains the coating 210Y. This is because the coating 210Y can be easily formed and the surface of the core 210X is sufficiently protected electrochemically by the coating 210Y.
[0054] Here, as will be described later, the covering portion 210Y is formed on the surface of the central portion 210X using a covering source material during the manufacturing process of the secondary battery, more specifically, during a stabilization treatment (initial charge / discharge treatment) of the secondary battery after assembly. In this case, the covering source material decomposes and reacts during the stabilization treatment, so that the covering portion 210Y is formed so as to cover the surface of the central portion 210X.
[0055] This coating source material is a material containing a constituent element of the coating portion 210Y, and more specifically, is one or more of materials that serve as a supply source of boron and fluorine contained as constituent elements in the coating portion 210Y. The location where the coating source material exists is not particularly limited as long as it is inside the secondary battery before the stabilization treatment.
[0056] The coating source material may be a material containing boron as a constituent element (boron-containing material) and a material containing fluorine as a constituent element (fluorine-containing material), or a material containing boron and fluorine as constituent elements (boron-fluorine-containing material).
[0057] Details such as the location and type of the coating source material will be described later.
[0058] The positive electrode binder contains one or more of materials such as synthetic rubber and polymer compounds. Specific examples of synthetic rubber include styrene-butadiene rubber, fluorine-containing rubber, and ethylene-propylene-diene. Specific examples of polymer compounds include polyvinylidene fluoride, polyimide, and carboxymethyl cellulose.
[0059] The positive electrode conductive agent contains one or more conductive materials such as a carbon material, a metal material, and a conductive polymer compound, and specific examples of the carbon material include graphite, carbon black, acetylene black, and ketjen black.
[0060] The other materials contained in the positive electrode active material layer 21B may further include one or more of the materials other than the above-mentioned positive electrode binder and positive electrode conductive agent.
[0061] Specifically, the other material is a dispersant used in the manufacturing process of the secondary battery (a process of preparing a cathode mixture slurry), which will be described later. This dispersant is a material that improves the dispersibility of the plurality of cathode active material particles 210 and the like in the cathode mixture slurry, and a specific example of the dispersant is polyvinylpyrrolidone.
[0062] The other material may be one or more of the coating source materials. A specific example of the coating source material used in the positive electrode 21 is lithium metaborate (LiBO), which is a boron-containing material. 2 ) and the like, and the coating source material is used to form the coating portion 210Y in the stabilization treatment of the secondary battery after assembly, as described above.
[0063] In this secondary battery, in order to improve the battery characteristics, predetermined conditions are met with respect to the physical properties of the positive electrode active material layer 21B. The physical properties of the positive electrode active material layer 21B will be described in detail later.
[0064] (Negative Electrode) As shown in FIG. 2, the negative electrode 22 includes a negative electrode current collector 22A and a negative electrode active material layer 22B.
[0065] The negative electrode current collector 22A has a pair of surfaces on which the negative electrode active material layer 22B is provided. The negative electrode current collector 22A contains a conductive material such as a metal material, and a specific example of the conductive material is copper.
[0066] The anode active material layer 22B contains a lithium-absorbing anode active material. However, the anode active material layer 22B may further contain one or more of other materials such as a anode binder and anode conductor. The method for forming the anode active material layer 22B is not particularly limited, but may be one or more of a coating method, a vapor phase method, a liquid phase method, a thermal spraying method, and a firing method (sintering method).
[0067] Here, the anode active material layer 22B is provided on both sides of the anode current collector 22A. However, the anode active material layer 22B may be provided on only one side of the anode current collector 22A on the side where the anode 22 faces the cathode 21.
[0068] The type of negative electrode active material is not particularly limited, but specific examples include carbon materials and metal-based materials, because high energy density can be obtained.
[0069] Specific examples of carbon materials include graphitizable carbon, non-graphitizable carbon, and graphite (natural graphite and artificial graphite).
[0070] A metal-based material is a material containing, as a constituent element, one or more of metal elements and metalloid elements that can form an alloy with lithium, and specific examples of the metal elements and metalloid elements include silicon and tin. This metal-based material may be a simple substance, an alloy, a compound, a mixture of two or more of these, or a material containing two or more of these phases. However, the "simple substance" described here may contain any amount of impurities, so the purity of the "simple substance" is not necessarily limited to 100%. A specific example of a metal-based material is TiSi 2 and SiO x (0<x≦2, or 0.2<x<1.4), etc.
[0071] The details regarding the negative electrode binder are the same as those regarding the positive electrode binder, and the details regarding the negative electrode conductive agent are the same as those regarding the positive electrode conductive agent.
[0072] 2, the separator 23 is an insulating porous film interposed between the positive electrode 21 and the negative electrode 22, and allows lithium to pass through in an ionic state while preventing the occurrence of a short circuit due to contact between the positive electrode 21 and the negative electrode 22. The separator 23 contains a polymer compound such as polyethylene.
[0073] (Electrolyte) The electrolyte is a liquid electrolyte that is impregnated into the positive electrode 21, the negative electrode 22, and the separator 23, and contains a solvent and an electrolyte salt.
[0074] Here, the solvent contains one or more types of non-aqueous solvents (organic solvents), and the electrolyte solution containing the non-aqueous solvent is a so-called non-aqueous electrolyte solution. The non-aqueous solvents include esters and ethers, more specifically, carbonate ester compounds, carboxylic acid ester compounds, and lactone compounds. This is because the dissociation of the electrolyte salt is improved and the mobility of ions is also improved.
[0075] The carbonate ester compounds include cyclic carbonate esters and chain carbonate esters. Specific examples of the cyclic carbonate esters include ethylene carbonate and propylene carbonate, and specific examples of the chain carbonate esters include dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate.
[0076] The carboxylic acid ester compound is a chain carboxylic acid ester, and specific examples of the chain carboxylic acid ester include ethyl acetate, ethyl propionate, propyl propionate, and ethyl trimethylacetate. The lactone compound is a lactone, and specific examples of the lactone include γ-butyrolactone and γ-valerolactone. The ether may be 1,2-dimethoxyethane, tetrahydrofuran, 1,3-dioxolane, or 1,4-dioxane.
[0077] The electrolyte salt contains one or more light metal salts such as lithium salts. Specific examples of lithium salts include lithium hexafluorophosphate (LiPF 6 ), lithium tetrafluoroborate (LiBF 4 ), lithium trifluoromethanesulfonate (LiCF 3 SO 3 ), lithium bis(fluorosulfonyl)imide (LiN(FSO 2 ) 2 ), lithium bis(trifluoromethanesulfonyl)imide (LiN(CF 3 SO 2 ) 2 ), lithium tris(trifluoromethanesulfonyl)methide (LiC(CF 3 SO 2 ) 3 ), lithium bis(oxalato)borate (LiB(C 2 O 4 ) 2 ), lithium monofluorophosphate (Li 2 PFO 3 ) and lithium difluorophosphate (LiPF 2 O 2 ) etc. This is because a high battery capacity can be obtained.
[0078] The content of the electrolyte salt is not particularly limited, but specifically, it is 0.3 mol / kg to 3.0 mol / kg relative to the solvent, because high ionic conductivity can be obtained.
[0079] The electrolyte solution may further contain one or more additives, which improves the electrochemical stability of the electrolyte solution. The additives are not particularly limited, but specific examples include unsaturated cyclic carbonates, fluorinated cyclic carbonates, sulfonates, phosphates, acid anhydrides, nitrile compounds, and isocyanate compounds.
[0080] Specific examples of unsaturated cyclic carbonates include vinylene carbonate, vinylethylene carbonate, and methyleneethylene carbonate. Specific examples of fluorinated cyclic carbonates include monofluoroethylene carbonate and difluoroethylene carbonate. Specific examples of sulfonic acid esters include propane sultone and propene sultone. Specific examples of phosphate esters include trimethyl phosphate and triethyl phosphate. Specific examples of acid anhydrides include succinic anhydride, 1,2-ethanedisulfonic anhydride, and 2-sulfobenzoic anhydride. Specific examples of nitrile compounds include succinonitrile. Specific examples of isocyanate compounds include hexamethylene diisocyanate.
[0081] The electrolyte may contain one or more of the coating source materials. Specific examples of the coating source material used in the electrolyte include lithium metaborate (LiBO), which is a boron-containing material. 2 ), and lithium hexafluorophosphate (LiPF), a fluorine-containing material. 6 ) and boron-fluorine-containing material lithium tetrafluoroborate (LiBF 4 As described above, this coating source material is used to form the coating portion 210Y in the stabilization treatment of the secondary battery after assembly.
[0082] 1 and 2, the positive electrode lead 31 is a positive electrode wiring connected to the positive electrode current collector 21A and is led out of the exterior film 10. The positive electrode lead 31 contains a conductive material such as a metal material, and a specific example of the conductive material is aluminum. The positive electrode lead 31 has a shape such as a thin plate or a mesh.
[0083] [Negative Electrode Lead] As shown in FIGS. 1 and 2 , the negative electrode lead 32 is a negative electrode wiring connected to the negative electrode current collector 22A, and is led out of the exterior film 10. Here, the lead-out direction of the negative electrode lead 32 is the same as the lead-out direction of the positive electrode lead 31. The negative electrode lead 32 contains a conductive material such as a metal material, and a specific example of the conductive material is copper. Note that the details regarding the shape of the negative electrode lead 32 are the same as the details regarding the shape of the positive electrode lead 31.
[0084] [Sealing Film] The sealing film 41 is inserted between the exterior film 10 and the positive electrode lead 31, and the sealing film 42 is inserted between the exterior film 10 and the negative electrode lead 32. However, one or both of the sealing films 41 and 42 may be omitted.
[0085] The sealing film 41 is a sealing member that prevents outside air and the like from entering the inside of the exterior film 10. This sealing film 41 contains a polymer compound such as polyolefin that has adhesiveness to the positive electrode lead 31, and a specific example of the polymer compound is polypropylene.
[0086] The configuration of the sealing film 42 is the same as the configuration of the sealing film 41, except that the sealing film 42 is a sealing member that has adhesiveness to the negative electrode lead 32. That is, the sealing film 42 contains a polymer compound such as polyolefin that has adhesiveness to the negative electrode lead 32.
[0087] <1-2. Physical Properties> As described above, in this secondary battery, in order to improve the battery characteristics, predetermined conditions are met regarding the physical properties of the positive electrode active material layer 21B. In the following, it is assumed that the covering portion 210Y is made of lithium fluoroborate (LiBOF 2 ) will be explained.
[0088] 4 shows the results of analysis of the positive electrode active material layer 21B in the depth direction D using time-of-flight secondary ion mass spectrometry (TOF-SIMS). In Fig. 4, the horizontal axis represents the sputtering time (seconds) and the vertical axis represents the ion intensity (counts).
[0089] [Physical Property Conditions When Positive Electrode Active Material Particles Contain a Coating Portion] The positive electrode active material layer 21B is analyzed in the depth direction D using TOF-SIMS. The analysis using TOF-SIMS described here is so-called depth analysis. Note that the depth direction D corresponds to the thickness direction of the positive electrode active material layer 21B as shown in FIG. 2 , and more specifically, it is the direction from the surface of the positive electrode active material layer 21B toward the inside of the positive electrode active material layer 21B.
[0090] In this depth analysis, normal ion analysis using primary ions and sputter etching, which uses sputter ions to dig into the positive electrode active material layer 21B, are alternately repeated in the depth direction D. This allows the amounts of various ions detected from the positive electrode active material layer 21B in the depth direction D to be measured, and therefore, an analysis result of the positive electrode active material layer 21B in the depth direction D is obtained, as shown in FIG.
[0091] As described above, the horizontal axis indicates the sputtering time during sputter etching, and therefore corresponds to the position (so-called depth) inside the positive electrode active material layer 21B in the depth direction D. Furthermore, as described above, the horizontal axis indicates the ion intensity, and therefore corresponds to the detected amount of each type of ion in the depth direction D.
[0092] As shown in FIG. 3, the positive electrode active material particle 210 includes a central portion 210X (lithium composite oxide with a content ratio C of 80 mol % or more) and a coating portion 210Y (lithium fluoroborate). In this case, two types of negative secondary ions are detected by analyzing the positive electrode active material layer 21B in the depth direction D using TOF-SIMS. These two types of negative secondary ions are NiO2 - and a first negative secondary ion derived from LiBO 2 F - and second negative secondary ions derived from
[0093] As a result, as shown in Figure 4, a first depth profile 4A representing the change in ion intensity of the first negative secondary ion in the depth direction D and a second depth profile 4B representing the change in ion intensity of the second negative secondary ion in the depth direction D are obtained.
[0094] When the covering portion 210Y covers the surface of the central portion 210X and the covering portion 210Y contains lithium fluoroborate, the following three types of physical property conditions are met.
[0095] (First physical property condition) In the first depth profile 4A, the detected amount of the first negative secondary ions increases as the sputtering time increases, and therefore the ion intensity of the first negative secondary ions increases in the depth direction D. In this case, the ion intensity of the first negative secondary ions may increase suddenly in the middle of the depth direction D, i.e., in the middle of the increase in the ion intensity of the first negative secondary ions.
[0096] The reason why the ion intensity of the first negative secondary ions increases in the depth direction D will be explained below.
[0097] As described above, the positive electrode active material layer 21B contains not only the plurality of positive electrode active material particles 210 but also a positive electrode binder, a positive electrode conductor, and the like. A portion (the central portion 210X) of the positive electrode active material particles 210 contains a large amount of nickel as a constituent element, whereas the positive electrode binder, the positive electrode conductor, and the like contain almost no nickel as a constituent element. In this case, analysis of the positive electrode active material layer 21B in the depth direction D using TOF-SIMS detects first negative secondary ions in regions where nickel is sufficiently present, but does not detect first negative secondary ions in regions where nickel is almost absent.
[0098] As a result, when the positive electrode active material layer 21B is analyzed in the depth direction D using TOF-SIMS, as described above, the detected amount of the first negative secondary ions increases in the depth direction D, and therefore the ionic strength of the first negative secondary ions increases in the depth direction D.
[0099] In particular, when there are almost no positive electrode active material particles 210 near the outermost surface of the positive electrode active material layer 21B, the ionic strength of the first negative secondary ions increases gradually, whereas inside the positive electrode active material layer 21B, there is a large number of positive electrode active material particles 210, and therefore the ionic strength of the first negative secondary ions increases rapidly. As a result, the ionic strength of the first negative secondary ions increases gradually in the depth direction D and then increases rapidly, and as described above, the ionic strength of the first negative secondary ions may increase rapidly in the middle of the depth direction D.
[0100] (Second Physical Property Condition) In the second depth profile 4B, the detected amount of the second negative secondary ions decreases as the sputtering time increases, and therefore the ion intensity of the second negative secondary ions decreases in the depth direction D.
[0101] The reason why the ion intensity of the second negative secondary ions decreases in the depth direction D is as follows.
[0102] In the stabilization treatment of the assembled secondary battery, not only the coating source material but also multiple types of compounds present inside the assembled secondary battery decompose and react, so that a coating containing various decomposition products and reaction products is formed on the surface of the positive electrode active material layer 21B. Specific examples of the multiple types of compounds include the solvent and electrolyte salt contained in the electrolyte solution.
[0103] The various decomposition products and reaction products contained in the coating may contain large amounts of boron and fluorine as constituent elements. In contrast, the positive electrode binder and positive electrode conductor contained in the positive electrode active material layer 21B do not contain as many boron and fluorine as constituent elements as the above-mentioned coating. In this case, analysis of the positive electrode active material layer 21B in the depth direction D using TOF-SIMS detects second negative secondary ions in regions where boron and fluorine are sufficiently present, but does not detect second negative secondary ions in regions where boron and fluorine are hardly present.
[0104] As a result, when the positive electrode active material layer 21B is analyzed in the depth direction D using TOF-SIMS, as described above, the detected amount of the second negative secondary ions decreases in the depth direction D, and therefore the ionic strength of the second negative secondary ions decreases in the depth direction D.
[0105] (Third physical property condition) However, the second depth profile 4B has a step region S in which the ion intensity of the second negative secondary ions temporarily stops decreasing in the depth direction D while the ion intensity of the first negative secondary ions increases in the depth direction D.
[0106] In this step region S, the ionic strength of the second negative secondary ions may be constant in the depth direction D, or the ionic strength of the second negative secondary ions may increase in the depth direction D, or there may be a mixture of regions where the ionic strength of the second negative secondary ions is constant in the depth direction D and regions where the ionic strength of the second negative secondary ions increases in the depth direction D.
[0107] The reason why the second depth profile 4B has the step region S will be explained below.
[0108] As described above, in the stabilization treatment of the secondary battery after assembly, a coating is formed on the surface of the positive electrode active material layer 21B due to the decomposition and reaction of not only the coating source material but also multiple types of compounds, and therefore the ionic strength of the second negative secondary ions decreases in the depth direction D.
[0109] However, a portion (coating portion 210Y) of the positive electrode active material particle 210 contains lithium fluoroborate and therefore contains a large amount of boron and fluorine as constituent elements. In this case, analysis of the positive electrode active material layer 21B in the depth direction D using TOF-SIMS detects second negative secondary ions in regions where boron and fluorine are sufficiently present, but does not detect second negative secondary ions in regions where boron and fluorine are hardly present.
[0110] As a result, when the positive electrode active material layer 21B is analyzed in the depth direction D using TOF-SIMS, the ionic intensity of the second negative secondary ions decreases in the depth direction D, but when the analysis position in the depth direction D reaches the covering portion 210Y, the ionic intensity of the second negative secondary ions temporarily increases. As a result, the ionic intensity of the second negative secondary ions temporarily stops decreasing. After this, when the analysis position in the depth direction D reaches the center portion 210X, the ionic intensity of the second negative secondary ions decreases again. Therefore, the second depth profile 4B has a step region S where the ionic intensity of the second negative secondary ions temporarily stops decreasing midway in the depth direction D.
[0111] [Physical property conditions when the positive electrode active material particle does not include a coating portion] When the positive electrode active material particle 210 does not include the coating portion 210Y (lithium fluoroborate) but includes only the center portion 210X (lithium composite oxide having a content ratio C of 80 mol% or more), a first depth profile 4A is obtained, and a third depth profile 4C is obtained instead of the second depth profile 4B.
[0112] In FIG. 4, the first depth profile 4A and the second depth profile 4B are shown by solid lines, and the third depth profile 4C is shown by dashed lines.
[0113] In the third depth profile 4C, since the coating portion 210Y is not present inside the positive electrode active material layer 21B, the ionic strength of the second negative secondary ions decreases in the depth direction D. That is, since the ionic strength of the second negative secondary ions does not temporarily increase partway through the depth direction D, the ionic strength of the second negative secondary ions does not temporarily decrease partway through the depth direction D but decreases continuously in the depth direction D. As a result, the third depth profile 4C does not have a step region S, unlike the second depth profile 4B.
[0114] In addition, even if the positive electrode active material particle 210 includes a coating portion 210Y, if the amount of the coating portion 210Y formed is insufficient, a third depth profile 4C is obtained instead of the second depth profile 4B, just as in the case where the positive electrode active material particle 210 does not include the coating portion 210Y.
[0115] [Analysis Procedure] As described above, by analyzing the positive electrode active material layer 21B in the depth direction D using TOF-SIMS, it is possible to identify after the fact (after the secondary battery is completed) that the positive electrode active material particle 210 includes the central portion 210X (lithium composite oxide having a content ratio C of 80 mol % or more) and the coating portion 210Y (lithium fluoroborate).
[0116] In other words, by analyzing the positive electrode active material layer 21B in the depth direction D using TOF-SIMS, if the above-mentioned three types of physical property conditions are met, it is demonstrated that the positive electrode active material particle 210 includes the central portion 210X (lithium composite oxide having a content ratio C of 80 mol % or more) and the coating portion 210Y (lithium fluoroborate).
[0117] Here, as the TOF-SIMS analyzer, a TOF-SIMS V manufactured by ION-TOF can be used. The analysis conditions are as follows: primary ion = Bi 3+ , ion gun acceleration voltage = 25 keV, analysis mode = depth profile analysis by high current bunching, irradiated ion current (measured with pulsed beam) = 0.2 pA, pulse frequency = 10 kHz, mass range = 1 amu to 800 amu, scanning range = 200 μm × 200 μm, sputter ions = Ar + The acceleration voltage of the sputter ion gun is 1 kV, the emission current is 200 mA, and the sputter area is 500 μm×500 μm.
[0118] The procedure for analyzing the positive electrode active material layer 21B in the depth direction D using TOF-SIMS to confirm whether or not the three physical property conditions are met is as follows.
[0119] First, the secondary battery is discharged until the voltage reaches 2.0 V. The current during discharge is not particularly limited and can be set arbitrarily.
[0120] Next, the secondary battery is disassembled in a glove box to recover the positive electrode 21, and then the positive electrode 21 is washed with a washing solvent, thereby removing the electrolyte impregnated in the positive electrode 21. The type of washing solvent is not particularly limited, but specifically, it is any one or more types of organic solvents such as dimethyl carbonate.
[0121] Next, the cleaned positive electrode 21 is attached to a sample holder using adhesive tape. The type of adhesive tape is not particularly limited, but specifically, carbon tape or the like is used. Next, the positive electrode active material layer 21B is analyzed in the depth direction D using TOF-SIMS, thereby obtaining the analysis results shown in FIG.
[0122] Finally, based on the analysis results, it is visually confirmed whether or not the three physical property conditions are met.
[0123] Specifically, since the ionic strength of the first negative secondary ions increases in the depth direction D, when the first depth profile 4A is acquired, a plurality of positive electrode active material particles 210 (a central portion 210X containing a lithium composite oxide having a content ratio C of 80 mol% or more) are present inside the positive electrode active material layer 21B, and therefore the first physical property condition is met.
[0124] Furthermore, since the ion intensity of the second negative secondary ions decreases in the depth direction D, when the second depth profile 4B is acquired, the second physical property condition is met.
[0125] Furthermore, even if the ionic strength of the second negative secondary ions decreases in the depth direction D, when the second depth profile 4B has a step region S, multiple positive electrode active material particles 210 (coating portion 210Y containing lithium fluoroborate) are present inside the positive electrode active material layer 21B, and therefore the third physical property condition is satisfied.
[0126] In addition, if a third depth profile 4C that does not have a step region S is obtained instead of the second depth profile 4B that has the step region S, the second physical property condition is not met because the positive electrode active material particle 210 does not include the coating portion 210Y, or even if the positive electrode active material particle 210 includes the coating portion 210Y, the amount of the coating portion 210Y formed is insufficient.
[0127] [Reason for Using TOF-SIMS as an Analytical Method] The reason for using TOF-SIMS (depth analysis) as an analytical method for investigating the physical properties of the positive electrode active material layer 21B is as follows.
[0128] First, the thickness of the covering portion 210Y is assumed to be extremely thin, being on the order of several nanometers. In this case, in order to examine the physical properties of the positive electrode active material layer 21B in the depth direction D, it is effective to employ TOF-SIMS (depth analysis), which has extremely high depth resolution.
[0129] Second, when multiple types of compounds are present inside the positive electrode active material layer 21B, it is more effective to use TOF-SIMS, which can examine the compositions of the multiple types of compounds individually, rather than using an analytical method which can examine the average composition of the positive electrode active material layer 21B.
[0130] Specifically, in general, when investigating the composition of a coating, analytical methods such as X-ray photoelectron spectroscopy (XPS) and electron energy loss spectroscopy (TEM-EELS) are used.
[0131] However, in XPS, the spectrum derived from boron and the spectrum derived from phosphorus overlap each other, making it difficult to examine the chemical bonding state of the boron, and even to examine the presence or absence of boron.
[0132] Furthermore, in TEM-EELS (particle cross-sectional analysis), when a line analysis of a coating is performed in the depth direction D, an average composition containing lithium, boron, oxygen, and fluorine is analyzed in a state in which not only lithium fluoroborate but also other compounds are contained, making it difficult to analyze only the lithium fluoroborate.
[0133] In contrast, TOF-SIMS analyzes the average composition of lithium fluoroborate alone, which contains lithium, boron, oxygen, and fluorine, and therefore makes it possible to analyze only the lithium fluoroborate.
[0134] Third, in surface analysis using TOF-SIMS, it is possible to analyze the various ions present on the surface of the coating, but it is difficult to analyze the various ions present inside the coating.
[0135] In contrast, depth analysis using TOF-SIMS not only makes it possible to analyze various ions present on the surface of the coating, but also to analyze various ions present inside the coating, thereby making it possible to analyze various ions related to the positive electrode active material layer 21B, and more specifically, to analyze various ions present inside the coating portion 210Y provided on the surface of the center portion 210X.
[0136] <1-3. Operation> The secondary battery operates in the battery element 20 as follows.
[0137] During charging, lithium is released from the positive electrode 21 and is absorbed into the negative electrode 22 via the electrolyte. During discharging, lithium is released from the negative electrode 22 and is absorbed into the positive electrode 21 via the electrolyte. During discharging and charging, lithium is absorbed and released in an ionic state.
[0138] <1-4. Manufacturing Method> When manufacturing a secondary battery, the positive electrode 21 and the negative electrode 22 are fabricated and an electrolytic solution is prepared according to the procedure described below as an example. Thereafter, the positive electrode 21, the negative electrode 22, and the electrolytic solution are used to assemble a secondary battery, and a stabilization process is performed on the assembled secondary battery.
[0139] The following describes a method for manufacturing a secondary battery in which the covering portion 210Y contains lithium fluoroborate.
[0140] [Fabrication of Positive Electrode] First, a plurality of cores 210X containing a lithium composite oxide (content ratio C≧80 mol%) are prepared. This lithium composite oxide contains residual alkaline components therein, and the residual alkaline components are lithium hydroxide (LiOH) and lithium carbonate (Li 2 CO 3 The remaining alkaline components are mainly present at the grain boundaries inside the lithium composite oxide.
[0141] Next, the plurality of central portions 210X are heated in a pressurized environment. The heating conditions, such as the pressure (Pa) in the environment, the heating temperature (°C), and the heating time (hours), can be set as desired. As a result, the remaining alkaline components contained in the central portions 210X are heated, and the remaining alkaline components are diffused to the surface of the central portions 210X. Therefore, the remaining alkaline components tend to be uniformly present on the surface of the central portions 210X.
[0142] Here, by heating the central portion 210X, the remaining alkaline components are diffused onto the surface of the central portion 210X, because the coating portion 210Y is more easily formed by utilizing the reaction between the remaining alkaline components and the coating source material during the stabilization process of the secondary battery after assembly, which will be described later.
[0143] The content (wt %) of the remaining alkali component in the central portion 210X is not particularly limited as long as the coating portion 210Y is formed using the remaining alkali component. The content of the remaining alkali component is calculated based on the following formula: content of remaining alkali component = (weight of remaining alkali component / weight of central portion 210X) x 100. In this case, the amount of the remaining alkali component diffused onto the surface of the central portion 210X can be controlled by changing the heating conditions.
[0144] The procedure for calculating the content of the residual alkali component in the central portion 210X is as follows. First, the weight M1 of the multiple central portions 210X is measured. Next, the weight M2 of the residual alkali component contained in the multiple central portions 210X is measured using the two-stage neutralization titration method (Walder method) described below. Finally, the content of the residual alkali component is calculated based on the above-mentioned formula.
[0145] The procedure for measuring the weight M2 of the remaining alkali component using the two-stage neutralization titration method is as follows.
[0146] The weight M2 of the remaining alkaline component is the weight of the remaining alkaline component contained in the supernatant of the remaining alkaline aqueous solution, and more specifically, the total weight of lithium hydroxide and lithium carbonate.
[0147] Since the supernatant of the residual alkaline aqueous solution is an aqueous solution containing the residual alkaline component, the weight M2 of the residual alkaline component can be measured based on the amount of acid titrated to neutralize the supernatant until the neutralization point is reached. In this case, the residual alkaline aqueous solution may be diluted with pure water. The neutralization point in the neutralization titration is determined using electrotitration. In this electrotitration, the point at which the rate of change in measured potential relative to the amount of acid titrated is the largest is the first neutralization point (final neutralization point), and the point at which the rate of change in measured potential relative to the amount of acid titrated is the second largest is the first neutralization point.
[0148] In the neutralization titration, hydrochloric acid (concentration = 0.1 mol / l (= 0.1 mol / dm 3 )) may be used. In this case, the neutralization reactions shown in reaction formulas (1) to (3) proceed, and the weight M2 of the remaining alkali component can be calculated using calculation formula (4). Reaction formulas (1) and (2) show the neutralization reactions that proceed up to the first neutralization point, and reaction formula (3) shows the neutralization reaction that proceeds from the first neutralization point to the second neutralization point.
[0149] LiOH+HCl → LiCl+H 2 O...(1) Li 2 CO 3 +HCl → LiCl+LiHCO 3 ...(2) LiHCO 3 ++HCl → LiCl+CO 2 +H 2 O...(3) M2=cf(V2-V1)m1+cf(2V1-V2)m2...(4)
[0150] In calculation formula (4), M2 represents the weight of the remaining alkali component, c represents the concentration of hydrochloric acid used in the neutralization titration, f represents a factor value of hydrochloric acid used in the neutralization titration (a coefficient for correcting the concentration of hydrochloric acid), V1 represents the volume of hydrochloric acid required up to the first neutralization point, V2 represents the volume of hydrochloric acid required up to the second neutralization point, m1 represents the molecular weight of lithium carbonate, and m2 represents the molecular weight of lithium hydroxide.
[0151] Next, the heated positive electrode active material particles 210, the positive electrode binder, and the positive electrode conductive agent are mixed together to form a positive electrode mixture. Next, the positive electrode mixture is poured into a solvent to prepare a paste-like positive electrode mixture slurry. This solvent may be an aqueous solvent or an organic solvent.
[0152] Next, a precursor layer (not shown) is formed by applying the cathode mixture slurry to both surfaces of the cathode current collector 21A. This precursor layer has a configuration similar to that of the cathode active material layer 21B, except that the coating portion 210Y is not provided on the surface of the center portion 210X and the precursor layer is not impregnated with an electrolyte solution. The precursor layer may then be compression-molded using a roll press or the like. In this case, the precursor layer may be heated, or the compression molding of the precursor layer may be repeated multiple times.
[0153] Finally, as described below, after assembling the secondary battery, a stabilization process is performed using the assembled secondary battery. As a result, the coating portion 210Y is formed on the surface of the center portion 210X, thereby forming the positive electrode active material particles 210. Thus, the positive electrode active material layer 21B containing the plurality of positive electrode active material particles 210 is formed, thereby producing the positive electrode 21.
[0154] When a coating source material is used in the process of producing the positive electrode 21, the positive electrode 21 is produced by the procedure described below.
[0155] First, the plurality of central portions 210X are mixed with a powdered coating source material. As described above, this coating source material includes a boron-containing material such as lithium metaborate. This causes the powdered coating source material to adhere to the surfaces of the central portions 210X. As described above, this coating source material adhered to the surfaces of the central portions 210X will be used to form the coating portions 210Y in a subsequent process.
[0156] Next, a positive electrode mixture slurry is prepared by the above-described procedure using the plurality of central parts 210X having the powdered coating source material attached to the surface, and then a precursor layer is formed using the positive electrode mixture slurry.
[0157] Finally, after assembling the secondary battery, a stabilization process is performed using the assembled secondary battery. As a result, the powdered coating source material attached to the surface of the central portion 210X is used to form the coating portion 210Y on the surface of the central portion 210X, thereby forming the positive electrode active material layer 21B. Thus, the positive electrode active material layer 21B containing the plurality of positive electrode active material particles 210 is formed, and the positive electrode 21 is produced.
[0158] [Fabrication of Negative Electrode] First, a negative electrode active material, a negative electrode binder, and a negative electrode conductive agent are mixed together to form a negative electrode mixture. Next, the negative electrode mixture is poured into a solvent to prepare a paste-like negative electrode mixture slurry. Details regarding the solvent are as described above. Finally, the negative electrode mixture slurry is applied to both surfaces of the negative electrode current collector 22A to form the negative electrode active material layer 22B. Thereafter, the negative electrode active material layer 22B may be compression-molded using a roll press or the like. In this case, the negative electrode active material layer 22B may be heated, or the compression molding of the negative electrode active material layer 22B may be repeated multiple times. In this manner, the negative electrode 22 is fabricated.
[0159] [Preparation of Electrolyte Solution] An electrolyte salt is added to a solvent, whereby the electrolyte salt is dispersed or dissolved in the solvent, thereby preparing an electrolyte solution.
[0160] When a coating source material is used in the preparation of the electrolyte solution, an electrolyte salt that also serves as the coating source material may be used. As described above, the electrolyte salt that also serves as the coating source material contains a fluorine-containing material such as lithium hexafluorophosphate.
[0161] Furthermore, when a coating source material is used in the preparation of the electrolyte solution, the coating source material may be added to a solvent after the electrolyte salt has been introduced into the solvent. As described above, the coating source material contains a boron-containing material such as lithium tetrafluoroborate. This allows the coating source material to be dispersed or dissolved in the solvent, thereby preparing an electrolyte solution containing the coating source material. The coating source material contained in this electrolyte solution is used to form the coating portion 210Y in the stabilization treatment of the secondary battery after assembly.
[0162] [Assembly of Secondary Battery] First, the positive electrode lead 31 is connected to the positive electrode current collector 21A of the positive electrode 21 using a joining method such as welding, and the negative electrode lead 32 is connected to the negative electrode current collector 22A of the negative electrode 22 using a joining method such as welding.
[0163] Next, the positive electrode current collector 21A on which the precursor layer is formed and the negative electrode current collector 22A on which the negative electrode active material layer 22B is formed are stacked together with the separator 23 interposed therebetween to form a laminate (not shown). Next, the laminate is wound to form a wound body (not shown), and the wound body is then pressed using a press or the like to form a flat shape. This formed wound body has a configuration similar to that of the battery element 20, except that it contains the precursor layer instead of the positive electrode active material layer 21B and is not impregnated with an electrolyte solution.
[0164] Next, after the roll is housed inside the recess 10U, the exterior film 10 (fusion layer / metal layer / surface protection layer) is folded to face each other. Next, the outer peripheral edges of two sides of the facing fusion layers are bonded to each other using an adhesive method such as heat fusion, thereby housing the roll inside the bag-shaped exterior film 10.
[0165] Finally, after injecting the electrolyte solution into the bag-shaped exterior film 10, the outer peripheral edges of the remaining sides of the opposing fusion layers are bonded to each other using an adhesive method such as heat fusion. In this case, a sealing film 41 is inserted between the exterior film 10 and the positive electrode lead 31, and a sealing film 42 is inserted between the exterior film 10 and the negative electrode lead 32.
[0166] As a result, the wound body is impregnated with the electrolyte and is sealed inside the bag-shaped exterior film 10, thereby assembling a secondary battery.
[0167] [Stabilization Treatment of Assembled Secondary Battery] The assembled secondary battery is charged and discharged under various conditions, such as the ambient temperature, the number of charge / discharge cycles (number of cycles), and the charge / discharge conditions.
[0168] As a result, the coating portion 210Y is formed on the surface of the center portion 210X, thereby forming the positive electrode active material particle 210. Thus, the positive electrode active material layer 21B including the plurality of positive electrode active material particles 210 is formed, and the positive electrode 21 is fabricated.
[0169] Furthermore, since a coating is formed on the surface of the positive electrode 21, the positive electrode 21 is electrochemically stabilized, and since a coating is formed on the surface of the negative electrode 22, the negative electrode 22 is electrochemically stabilized.
[0170] Here, when a boron-containing material such as lithium metaborate is used as the coating source material (boron-containing material) in the manufacturing process of the positive electrode 21, and when lithium hexafluorophosphate is used as the electrolyte salt that also serves as the coating source material (fluorine-containing material) in the preparation process of the electrolyte solution, a coating portion 210Y containing lithium fluoroborate is formed by utilizing the reaction between the coating source materials described below.
[0171] LiBO 2 + LiPF 6 → LiBOF 2 +POF 3 +LiF
[0172] Furthermore, when lithium tetrafluoroborate is used as the coating source material (boron-fluorine-containing material) in the electrolyte solution preparation process, the coating portion 210Y containing lithium tetrafluoroborate is formed by utilizing the reaction between the coating source material and the remaining alkaline component described below.
[0173] LiBF 4 +Li 2 CO 3 → LiBOF 2 +2LiF+CO2 LiBF 4 +2LiOH → LiBOF 2 +2LiF+H 2 O
[0174] From these, the battery element 20 is produced and sealed inside the bag-shaped exterior film 10, thereby completing the secondary battery.
[0175] <1-5. Actions and Effects> In this secondary battery, the cathode active material layer 21B includes a plurality of cathode active material particles 210, each of which includes a central portion 210X and a coating portion 210Y, and the central portion 210X includes a lithium composite oxide (content ratio C≧80 mol%). Furthermore, with respect to the results of analysis of the cathode active material layer 21B in the depth direction D using TOF-SIMS, the above-described three types of physical property conditions are met.
[0176] In this case, since the central portion 210X contains a lithium composite oxide (content ratio C≧80 mol %), a high battery capacity can be obtained as described above.
[0177] Furthermore, because the coating portion 210Y is provided on the surface of the central portion 210X and the three physical property conditions regarding the physical properties of the positive electrode active material layer 21B are satisfied, as described above, even if the central portion 210X contains a lithium composite oxide (content ratio C≧80 mol%), the surface of the central portion 210X is electrochemically protected by the coating portion 210Y. Therefore, the charge transfer reaction is prevented from being inhibited, and oxidative decomposition of the electrolyte on the surface of the central portion 210X is also prevented, making it difficult for the electrical resistance of the positive electrode 21 to increase. As a result, the battery capacity is less likely to decrease even with repeated charging and discharging.
[0178] From these facts, even if a lithium composite oxide (content ratio C≧80 mol%) is used as the material for forming the central portion 210X, not only can a high battery capacity be obtained, but also excellent battery characteristics can be obtained because the electrical resistance of the positive electrode 21 is less likely to increase by using the coating portion 210Y.
[0179] In particular, if the coating portion 210Y contains lithium, boron, and fluorine as constituent elements, the coating portion 210Y is easily formed, and thus a higher effect can be obtained. In this case, if the coating portion 210Y contains lithium fluoroborate, the surface of the center portion 210X is sufficiently electrochemically protected by the coating portion 210Y, and thus an even higher effect can be obtained.
[0180] Furthermore, if the lithium composite oxide contains, as other elements, one or more of cobalt, aluminum, manganese, zirconium, titanium, molybdenum, tantalum, chromium, niobium, iron, copper, zinc, vanadium, magnesium, tungsten, sulfur, strontium, boron, sodium, and fluorine, a sufficient battery capacity can be obtained, thereby achieving a higher effect.
[0181] Furthermore, if the secondary battery is a lithium ion secondary battery, a sufficient battery capacity can be stably obtained by utilizing the absorption and release of lithium, and therefore a greater effect can be obtained.
[0182] 2. Modifications The configuration of the secondary battery can be modified as appropriate, as described below. However, any two or more of the series of modifications described below may be combined with each other.
[0183] [Variation 1] The case where the coating source material is contained in the positive electrode 21 or the electrolyte solution has been described. However, the location where the coating source material is contained is not particularly limited, and the coating source material may be contained in the negative electrode 22, or in two or more of the positive electrode 21, the negative electrode 22, and the electrolyte solution.
[0184] In this case, the covering portion 210Y is formed in the stabilization process of the secondary battery after assembly, so the same effect can be obtained.
[0185] [Modification 2] The case where the covering portion 210Y is formed after the secondary battery is assembled by using a stabilization treatment for the assembled secondary battery has been described. However, the covering portion 210Y may be formed before the secondary battery is assembled by forming the covering portion 210Y without using the stabilization treatment.
[0186] The procedure for producing the positive electrode 21 in the case where the covering portion 210Y is formed before assembling the secondary battery without using the stabilization treatment is as follows.
[0187] First, a treatment solution is prepared by mixing the material for forming the coating portion 210Y with a dispersion solvent. The material for forming the coating portion 210Y is a material that enables the three physical property conditions for the positive electrode active material layer 21B to be satisfied, and specifically, is the above-mentioned lithium fluoroborate. The type of dispersion solvent is not particularly limited and may be an aqueous solvent or an organic solvent.
[0188] When preparing the treatment solution, the treatment solution may contain a binder. Details regarding the binder are the same as those regarding the positive electrode binder.
[0189] Next, a treatment solution is applied to the surfaces of the plurality of central parts 210X, and then the treatment solution is dried to form the covering parts 210Y. In this case, instead of applying the treatment solution to the surfaces of the plurality of central parts 210X, the plurality of central parts 210X may be immersed in the treatment solution, and then the plurality of central parts 210X may be removed from the treatment solution and dried.
[0190] As a result, coating portions 210Y are formed on the surfaces of the plurality of central portions 210X, and thus a plurality of positive electrode active material particles 210 are formed.
[0191] Finally, the cathode active material layer 21B is formed by the above-described procedure using the plurality of cathode active material particles 210. In this way, the cathode 21 is produced without using a stabilization treatment for the secondary battery after assembly.
[0192] In this case as well, the positive electrode active material particle 210 including the central portion 210X and the coating portion 210Y is obtained, and therefore the same effect can be obtained.
[0193] [Modification 3] A porous film separator 23 is used. However, although not specifically shown here, a laminated separator including a polymer compound layer may be used instead of the porous film separator 23.
[0194] Specifically, the laminated separator includes a porous membrane having a pair of surfaces and a polymer compound layer provided on one or both surfaces of the porous membrane. This is because the separator's adhesion to the positive electrode 21 and the negative electrode 22 is improved, thereby suppressing misalignment of the battery element 20, i.e., miswinding of the positive electrode 21, the negative electrode 22, and the separator. This suppresses swelling of the secondary battery even if a decomposition reaction of the electrolyte occurs. The polymer compound layer includes a polymer compound such as polyvinylidene fluoride. Polyvinylidene fluoride has excellent physical strength and is electrochemically stable.
[0195] One or both of the porous film and the polymer compound layer may contain one or more types of insulating particles. This is because the insulating particles dissipate heat when the secondary battery generates heat, improving the safety (heat resistance) of the secondary battery. The insulating particles contain one or more types of insulating materials, such as inorganic materials and resin materials. Examples of inorganic materials include aluminum oxide, aluminum nitride, boehmite, silicon oxide, titanium oxide, magnesium oxide, and zirconium oxide. Examples of resin materials include acrylic resin and styrene resin.
[0196] When a laminated separator is produced, a precursor solution containing a polymer compound and an organic solvent is prepared, and then the precursor solution is applied to one or both sides of a porous film. In this case, the precursor solution may contain a plurality of insulating particles.
[0197] Even when this laminated separator is used, the same effect can be obtained because lithium can move in an ionic state between the positive electrode 21 and the negative electrode 22. In this case, as described above, in particular, the displacement of the battery element 20 is suppressed, thereby further suppressing swelling of the secondary battery, thereby achieving a greater effect.
[0198] [Modification 4] An electrolytic solution that is a liquid electrolyte is used. However, although not specifically shown here, an electrolyte layer that is a gel electrolyte may also be used.
[0199] In the battery element 20 using the electrolyte layer, the positive electrode 21 and the negative electrode 22 are wound facing each other with the separator 23 and the electrolyte layer interposed therebetween. The electrolyte layer is interposed between the positive electrode 21 and the separator 23, and also between the negative electrode 22 and the separator 23.
[0200] Specifically, the electrolyte layer contains a polymer compound together with an electrolytic solution, and the electrolytic solution is held by the polymer compound. This is because leakage of the electrolytic solution is prevented. The composition of the electrolytic solution is as described above. The polymer compound contains polyvinylidene fluoride, etc. When forming the electrolyte layer, a precursor solution containing the electrolytic solution, the polymer compound, a solvent, etc. is prepared, and then the precursor solution is applied to one or both surfaces of the positive electrode 21 and one or both surfaces of the negative electrode 22.
[0201] Even when this electrolyte layer is used, the same effect can be obtained because lithium can move in an ionic state through the electrolyte layer between the positive electrode 21 and the negative electrode 22. In this case, leakage of the electrolyte solution is particularly prevented as described above, and therefore a greater effect can be obtained.
[0202] 3. Uses of Secondary Batteries Finally, uses (application examples) of secondary batteries will be described.
[0203] The use of the secondary battery is not particularly limited. The secondary battery used as a power source may be a main power source or an auxiliary power source in electronic devices, electric vehicles, etc. The main power source is a power source that is used preferentially regardless of the presence or absence of other power sources. The auxiliary power source may be a power source used in place of the main power source or a power source that can be switched from the main power source.
[0204] Specific examples of uses for secondary batteries are as follows: Electronic devices such as video cameras, digital still cameras, mobile phones, laptop computers, headphone stereos, portable radios, and portable information terminals; Storage devices such as backup power supplies and memory cards; Power tools such as power drills and power saws; Battery packs installed in electronic devices; Medical electronic devices such as pacemakers and hearing aids; Electric vehicles such as electric cars (including hybrid cars); Power storage systems such as home or industrial battery systems that store power in preparation for emergencies, etc. In these uses, one secondary battery may be used, or multiple secondary batteries may be used.
[0205] The battery pack may include a single cell or a battery pack. The electric vehicle is a vehicle that runs on a secondary battery as a driving power source, and may be a hybrid vehicle that also includes a driving source other than the secondary battery. In a home power storage system, power stored in a secondary battery, which is a power storage source, can be used to power home electrical appliances, etc.
[0206] Here, an example of the use of the secondary battery will be specifically described. The configuration described below is merely an example and can be modified as appropriate.
[0207] Figure 5 shows the block diagram of a battery pack, which is an example of an application of a secondary battery. The battery pack described here is a battery pack (a so-called soft pack) that uses a single secondary battery, and is installed in electronic devices such as smartphones.
[0208] 5, the battery pack includes a power supply 51 and a circuit board 52. The circuit board 52 is connected to the power supply 51 and includes a positive terminal 53, a negative terminal 54, and a temperature detection terminal 55.
[0209] The power source 51 includes one secondary battery. The positive electrode lead of this secondary battery is connected to a positive electrode terminal 53, and the negative electrode lead is connected to a negative electrode terminal 54. The power source 51 is connected to the outside via the positive electrode terminal 53 and the negative electrode terminal 54, and is therefore capable of charging and discharging. The circuit board 52 includes a control unit 56, a switch 57, a PTC element 58 which is a thermosensitive resistor, and a temperature detection unit 59. However, the PTC element 58 may be omitted.
[0210] The control unit 56 includes a central processing unit (CPU) and memory, and controls the operation of the entire battery pack. The control unit 56 detects and controls the usage state of the power source 51.
[0211] When the voltage of power supply 51 (secondary battery) reaches the overcharge detection voltage or the overdischarge detection voltage, control unit 56 turns off switch 57 to prevent charging current from flowing through the current path of power supply 51. The overcharge detection voltage is not particularly limited, but specifically, it is 4.20 V±0.05 V, and the overdischarge detection voltage is not particularly limited, but specifically, it is 2.40 V±0.10 V.
[0212] Switch 57 includes a charge control switch, a discharge control switch, a charging diode, a discharging diode, etc., and switches between the connection and disconnection of power supply 51 and an external device in response to instructions from control unit 56. Switch 57 includes a metal oxide semiconductor field effect transistor (MOSFET), etc., and the charge current and the discharge current are detected based on the ON resistance of switch 57.
[0213] Temperature detection unit 59 includes a temperature detection element such as a thermistor. Temperature detection unit 59 measures the temperature of power supply 51 using temperature detection terminal 55 and outputs the temperature measurement result to control unit 56. The temperature measurement result measured by temperature detection unit 59 is used when control unit 56 controls charging and discharging in the event of abnormal heat generation, and when control unit 56 performs correction processing when calculating the remaining capacity.
[0214] An embodiment of the present technology will be described.
[0215] Examples 1 to 4 and Comparative Examples 1 to 3 Secondary batteries were manufactured as described below, and then the battery characteristics of the secondary batteries were evaluated. Here, test secondary batteries were used to evaluate the battery characteristics, as described below.
[0216] [Fabrication of Secondary Battery] FIG. 6 shows a cross-sectional structure of a test secondary battery, which is a so-called coin-type secondary battery (lithium ion secondary battery).
[0217] This secondary battery includes a test electrode 61, a counter electrode 62, a separator 63, an exterior cup 64, an exterior can 65, a gasket 66, and an electrolyte (not shown).
[0218] The test electrode 61 is housed in an exterior cup 64, and the counter electrode 62 is housed in an exterior can 65. The test electrode 61 and the counter electrode 62 are stacked together with a separator 63 interposed therebetween, and the test electrode 61, the counter electrode 62, and the separator 63 are impregnated with an electrolyte. The exterior cup 64 and the exterior can 65 are crimped together with a gasket 66, so that the test electrode 61, the counter electrode 62, and the separator 63 are sealed by the exterior cup 64 and the exterior can 65.
[0219] The secondary battery shown in FIG. 6 was fabricated according to the procedure described below.
[0220] (Preparation of Test Electrodes) First, a plurality of cores containing a lithium composite oxide (content ratio C≧80 mol%) were prepared. The composition of the lithium composite oxide, the content ratio C (mol%), and the content (wt%) of the residual alkaline component in the lithium composite oxide are as shown in Table 1.
[0221] Subsequently, the central portions were heated (heating temperature = 650°C and heating time = 10 hours) in a pressurized environment (pressure = 1 MPa).
[0222] Next, 95.5 parts by mass of the heated positive electrode active material particles, 2.5 parts by mass of a positive electrode binder (polyvinylidene fluoride), 1.9 parts by mass of a positive electrode conductive agent (carbon black), and 0.1 parts by mass of a dispersant (polyvinylpyrrolidone) were mixed together to prepare a positive electrode mixture. Next, the positive electrode mixture was added to a solvent (N-methyl-2-pyrrolidone, an organic solvent), and the solvent was stirred to prepare a paste-like positive electrode mixture slurry.
[0223] The positive electrode mixture slurry was then applied to one side of a positive electrode current collector (aluminum foil having a thickness of 15 μm), and the positive electrode mixture slurry was then heated and dried (heating temperature: 100° C. for 15 minutes) to form a precursor layer (thickness: 40 μm). The positive electrode current collector on which the precursor layer was formed was then punched out into a disk shape (diameter: 16.5 mm).
[0224] Finally, as described later, a secondary battery was assembled, and then the assembled secondary battery was subjected to a stabilization treatment. 2 ) was formed on the surface of the center portion, thereby forming positive electrode active material particles.
[0225] Thus, a positive electrode active material layer containing a plurality of positive electrode active material particles was formed, and thus a test electrode 61 was produced.
[0226] When a coating source material was used in the fabrication process of the test electrode 61, the multiple central portions were heated, and then a powdered boron-containing material (lithium metaborate) was added to the multiple central portions before the multiple central portions were used to obtain a positive electrode mixture. This mixture was then stirred. As a result, the powdered boron-containing material adhered to the surfaces of the central portions. The content of the coating source material (boron-containing material) in the mixture is as shown in Table 1. After this, a positive electrode mixture slurry was prepared using the multiple central portions with the boron-containing material adhered to their surfaces, and a precursor layer was formed using the positive electrode mixture slurry.
[0227] (Fabrication of Counter Electrode) A lithium metal plate was punched out into a disk shape (diameter = 17 mm), thereby obtaining a counter electrode 62.
[0228] (Preparation of Electrolyte Solution) A solvent (ethylene carbonate, which is a cyclic carbonate ester, and dimethyl carbonate, which is a chain carbonate ester) was mixed with an electrolyte salt (lithium hexafluorophosphate (LiPF )) which also served as a coating source material (fluorine-containing material). 6 The mixture ratio (weight ratio) of the solvent was ethylene carbonate:dimethyl carbonate = 30:70. The content of the electrolyte salt was 1 mol / L (= 1 mol / dm 3 ) Thus, the electrolyte solution was prepared.
[0229] When a coating source material is used in the preparation process of the electrolyte solution, the electrolyte solution may contain a boron-containing material (lithium tetrafluoroborate (LiBF 4 The content (wt %) of the coating source material (boron-containing material) in the electrolyte solution is shown in Table 1.
[0230] (Assembly of Secondary Battery) First, a test electrode 61 including a precursor layer was placed in an exterior cup 64, and a counter electrode 62 was placed in an exterior can 65. Next, the test electrode 61 placed in the exterior cup 64 and the counter electrode 62 placed in the exterior can 65 were stacked together with a separator 63 (a disc-shaped polyethylene film with a diameter of 17.5 μm) impregnated with an electrolyte interposed therebetween. In this case, the test electrode 61 was positioned so that the precursor layer and the counter electrode 62 faced each other with the separator 63 interposed therebetween. Next, with the test electrode 61 and the counter electrode 62 stacked together with the separator 63 interposed therebetween, the exterior cup 64 and the exterior can 65 were crimped together with a gasket 66. As a result, the test electrode 61 and the counter electrode 62 were enclosed by the exterior cup 64 and the exterior can 65, and a secondary battery was assembled.
[0231] (Stabilization Treatment of Assembled Secondary Battery) The assembled secondary battery was subjected to one cycle of charge and discharge.
[0232] During charging, the battery was first charged at a constant current of 0.1 C in a room temperature environment (temperature = 25°C) until the voltage reached 4.0 V. Subsequently, the battery was charged at a constant current of 0.1 C in a high temperature environment (temperature = 70°C) until the voltage reached 4.3 V. Finally, the battery was charged at a constant voltage of 4.3 V in a high temperature environment until the current reached 0.01 C.
[0233] During discharging, the battery was discharged at a constant current of 0.1 C in a room temperature environment until the voltage reached 2.5 V.
[0234] It should be noted that 0.1 C is a current value that completely discharges the battery capacity (theoretical capacity) in 10 hours, and 0.01 C is a current value that completely discharges the battery capacity in 100 hours.
[0235] As a result, coating portions were formed on the surfaces of the plurality of center portions, resulting in the formation of a plurality of positive electrode active material particles. Thus, a positive electrode active material layer containing the plurality of positive electrode active material particles was formed, thereby producing a test electrode 61, and thus a secondary battery was completed.
[0236] For comparison, a secondary battery was fabricated in the same manner except that no coating source material was used (excluding the electrolyte salt, which also served as the coating source material). In this case, the coating portion 210Y was not formed.
[0237] Here, after the secondary battery was completed, the physical properties (whether the three physical property conditions were met) were investigated based on the analysis results of depth analysis of the test electrode 61 using TOF-SIMS, and the results are shown in Table 1. Table 1 shows the type of coating source material other than the electrolyte salt that also serves as the coating source material, the location where the coating source material is contained, and the content (wt %) of the coating source material.
[0238] [Evaluation of Battery Characteristics] Electrical resistance characteristics were evaluated as battery characteristics according to the procedure described below, and the results shown in Table 1 were obtained.
[0239] To evaluate the electrical resistance characteristics, the secondary battery was first charged at a current of 0.1 C in a room temperature environment (temperature = 25 °C) until the voltage reached 4.25 V. Next, an impedance analyzer (Solartron Analytical AC Impedance Analyzer 1255WB) was used to perform electrochemical impedance spectroscopy (EIS) measurements on the charged secondary battery to obtain a Nyquist plot. In this case, the applied voltage was 10 mV, and the frequency range was 100 kHz to 0.1 Hz. Finally, the charge transfer resistance (charge transfer resistance (Ω) before cycling) of the test electrode 61 was measured based on the Nyquist plot (the arc on the low frequency side).
[0240] Subsequently, the secondary battery was repeatedly charged and discharged in the same environment until the total number of cycles reached 100. During charging, the battery was charged at a constant current of 1 C until the voltage reached 4.25 V, and then at the same voltage of 4.25 V, it was charged at a constant voltage of 0.01 C. During discharging, the battery was discharged at a constant current of 5 C until the voltage reached 2.5 V. 1 C is the current value at which the battery capacity is fully discharged in 1 hour, and 5 C is the current value at which the battery capacity is fully discharged in 0.2 hours.
[0241] Subsequently, the secondary battery was charged in the same environment at a current of 0.1 C until the voltage reached 4.25 V, and then the charge transfer resistance (charge transfer resistance (Ω) after cycling) of the test electrode 61 was calculated using the procedure described above.
[0242] Finally, the increase rate, which is an index for evaluating electrical resistance characteristics, was calculated based on the formula: Increase rate = [(charge transfer resistance after cycling - charge transfer resistance before cycling) / charge transfer resistance before cycling] x 100. This increase rate is a characteristic value that indicates how many times the charge transfer resistance after cycling has increased compared to the charge transfer resistance before cycling.
[0243]
[0244] [Discussion] As shown in Table 1, when a lithium composite oxide (content ratio C≧80 mol %) was used as the material for forming the central portion, the increase rate varied greatly depending on the physical properties of the positive electrode active material layer.
[0245] Specifically, even if a coating portion was formed using a coating source material, the first and second physical property conditions were met but the third physical property condition was not met due to an insufficient amount of the coating portion formed (Comparative Examples 1 and 2), and the increase rate increased significantly.
[0246] Similarly, in the case where the first and second physical property conditions were met but the third physical property condition was not met (Comparative Example 3), the increase rate also increased significantly because the coating portion was not formed due to the absence of the coating source material.
[0247] In contrast, when the coating portion was formed using the coating source material and the amount of the coating portion formed was sufficient so that not only the first and second physical property conditions were met but also the third physical property condition was met (Examples 1 to 4), the increase rate was significantly reduced.
[0248] In this case, the following trends were particularly observed. First, the increase rate was sufficiently reduced even when the content ratio C was changed. Second, the increase rate was sufficiently reduced even when the composition of the lithium composite oxide (the type of other elements) was changed. Third, when the coating portion contained lithium fluoroborate, the increase rate was significantly reduced.
[0249] [Summary] From the results shown in Table 1, the increase rate decreased when the positive electrode active material layer contained a plurality of positive electrode active material particles, the positive electrode active material particles included a core portion and a coating portion, the core portion contained a lithium composite oxide (content ratio C≧80 mol%), and three types of physical property conditions were met with respect to the results of analysis of the positive electrode active material layer 21B in the depth direction D using TOF-SIMS. Therefore, the electrical resistance characteristics were improved, and excellent battery characteristics were obtained in the secondary battery.
[0250] The present technology has been described above with reference to an embodiment and examples. However, the configuration of the present technology is not limited to the configuration described in the embodiment and examples, and can be modified in various ways.
[0251] Specifically, the battery structure of the secondary battery has been described as being a laminate film type and a coin type. However, the battery structure of the secondary battery is not particularly limited, and may be a cylindrical type, a square type, a button type, or the like.
[0252] The battery element has been described as having a wound structure. However, the structure of the battery element is not particularly limited, and may be a stacked structure or a zigzag structure. In the stacked structure, positive and negative electrodes are alternately stacked with a separator interposed therebetween, while in the zigzag structure, the positive and negative electrodes are folded in a zigzag pattern while facing each other with the separator interposed therebetween.
[0253] Although the electrode reactant is lithium in the above description, the electrode reactant is not particularly limited. Specifically, as described above, the electrode reactant may be other alkali metals such as sodium and potassium, or alkaline earth metals such as beryllium, magnesium, and calcium. Alternatively, the electrode reactant may be other light metals such as aluminum.
[0254] The effects described in this specification are merely examples, and the effects of the present technology are not limited to the effects described in this specification. Therefore, other effects may be obtained with respect to the present technology.
[0255] The present technology may also be configured as follows: <1> A cathode including a cathode active material layer, an anode, and an electrolyte solution, wherein the cathode active material layer includes a plurality of cathode active material particles, the cathode active material particles include a core including a lithium composite oxide and a coating portion provided on a surface of the core, the lithium composite oxide has a layered rock salt crystal structure and includes lithium, nickel, and other elements as constituent elements, and when the sum of the content of the nickel in the lithium composite oxide and the content of the other elements in the lithium composite oxide is taken as 100 parts by mol, the content of the nickel is 80 parts by mol or more and 100 parts by mol or less, and when an analysis of the cathode active material layer in the depth direction using time-of-flight secondary ion mass spectrometry reveals that NiO2 - a first negative secondary ion derived from LiBO; 2 F - and second negative secondary ions derived from the first negative secondary ions are detected, and a first depth profile representing a change in ionic intensity of the first negative secondary ions in the depth direction and a second depth profile representing a change in ionic intensity of the second negative secondary ions in the depth direction are acquired, wherein in the first depth profile, the ionic intensity of the first negative secondary ions increases in the depth direction, and in the second depth profile, the ionic intensity of the second negative secondary ions decreases in the depth direction, and the second depth profile has a step region where the ionic intensity of the second negative secondary ions temporarily stops decreasing in the depth direction while the ionic intensity of the first negative secondary ions increases in the depth direction. <2> The secondary battery according to <1>, wherein the coating portion contains lithium, boron, and fluorine as constituent elements. <3> The coating portion is made of lithium fluoroborate (LiBOF 2 <4> The secondary battery according to any one of <1> to <3>, wherein the other element includes at least one of cobalt, aluminum, manganese, zirconium, titanium, molybdenum, tantalum, chromium, niobium, iron, copper, zinc, vanadium, magnesium, tungsten, sulfur, strontium, boron, sodium, and fluorine. <5> The secondary battery according to any one of <1> to <4>, wherein the secondary battery is a lithium ion secondary battery.
[0256] 21... positive electrode, 21B... positive electrode active material layer, 22... negative electrode, 210... positive electrode active material particles, 210X... center portion, 210Y... coating portion
Claims
1. A method for manufacturing a lithium composite oxide comprising the steps of: a positive electrode including a positive electrode active material layer; a negative electrode; and an electrolyte; wherein the positive electrode active material layer includes a plurality of positive electrode active material particles; the positive electrode active material particles include a core including a lithium composite oxide and a coating portion provided on a surface of the core; the lithium composite oxide has a layered rock salt type crystal structure and includes lithium, nickel, and other elements as constituent elements; when the sum of the content of the nickel in the lithium composite oxide and the content of the other elements in the lithium composite oxide is taken as 100 parts by mole, the content of the nickel is 80 parts by mole or more and 100 parts by mole or less; and when an analysis of the positive electrode active material layer in the depth direction using time-of-flight secondary ion mass spectrometry reveals that NiO2 - A first negative secondary ion derived from LiBO 2 F - and second negative secondary ions derived from the first negative secondary ions are detected, and a first depth profile representing a change in ionic intensity of the first negative secondary ions in the depth direction and a second depth profile representing a change in ionic intensity of the second negative secondary ions in the depth direction are obtained, wherein in the first depth profile, the ionic intensity of the first negative secondary ions increases in the depth direction, and in the second depth profile, the ionic intensity of the second negative secondary ions decreases in the depth direction, and the second depth profile has a step region where the ionic intensity of the second negative secondary ions temporarily does not decrease in the depth direction while the ionic intensity of the first negative secondary ions is increasing in the depth direction.
2. The secondary battery according to claim 1, wherein the coating portion contains lithium, boron and fluorine as constituent elements.
3. The coating is made of lithium fluoroborate (LiBOF 2 The secondary battery according to claim 2 .
4. The secondary battery according to any one of claims 1 to 3, wherein the other elements include at least one of cobalt, aluminum, manganese, zirconium, titanium, molybdenum, tantalum, chromium, niobium, iron, copper, zinc, vanadium, magnesium, tungsten, sulfur, strontium, boron, sodium and fluorine.
5. The secondary battery according to any one of claims 1 to 4, which is a lithium ion secondary battery.
Citation Information
Patent Citations
Lithium ion secondary battery and manufacturing method therefor
JP2013062026A
Positive electrode active material particle including core containing lithium cobalt oxide and coating layer containing boron and fluorine, and preparation method thereof
US20180316015A1
Lithium ion secondary battery
WO2020209240A1
Secondary battery
WO2022196266A1