Lithium secondary battery
Patent Information
- Application Number
- PCT/JP2024/012666
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-03
Smart Images

Figure JP2024012666_03102024_PF_FP_ABST
Abstract
Description
Lithium secondary battery
[0001] The present disclosure relates to lithium secondary batteries.
[0002] Lithium ion batteries are known as high-capacity non-aqueous electrolyte secondary batteries. Lithium secondary batteries (lithium metal secondary batteries) are promising non-aqueous electrolyte secondary batteries with capacities even higher than lithium ion batteries. In lithium secondary batteries, lithium metal precipitates on the negative electrode during charging, and dissolves during discharging, releasing lithium ions into the non-aqueous electrolyte.
[0003] In lithium secondary batteries, lithium metal is deposited on the negative electrode during charging, so it is necessary to provide a space between the separator and the electrode to ensure a space for lithium to deposit.
[0004] Patent Document 1 proposes "a lithium secondary battery comprising: an electrode group in which a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode are wound; and a lithium ion conductive non-aqueous electrolyte; the negative electrode comprises a negative electrode current collector; the negative electrode current collector comprises a layer having a first surface facing outward from the winding of the electrode group and a second surface facing inward from the winding of the electrode group; a plurality of first protrusions protruding from the first surface; and a plurality of second protrusions protruding from the second surface; lithium metal is deposited on the first surface and the second surface by charging; and a second average height of the plurality of second protrusions is higher than the first average height of the plurality of first protrusions."
[0005] Patent Document 2 proposes "a sealed battery comprising a battery case including a cylindrical outer can with a bottom and a sealing body that closes the opening of the outer can, and an electrode body housed in the battery case, wherein the sealing body includes a metal plate, the metal plate having a thin-walled portion formed in an annular shape, a convex shape on the inside of the battery case, and an annular portion located outside the thin-walled portion that reverses to become convex on the outside of the case when the internal pressure of the battery case reaches a predetermined reversal pressure R, and the thin-walled portion is ruptured simultaneously with the reversal of the valve portion."
[0006] JP 2019-160776 A JP 2022-31997 A
[0007] Li deposited on the negative electrode during charging is highly reactive, and in the event of an internal short circuit or the like, the reaction rate of gas generation may shift to an accelerated mode, increasing the rate at which the internal battery pressure increases.
[0008] One aspect of the present disclosure relates to a lithium secondary battery including a power generating element and a battery case that seals the power generating element, wherein the power generating element includes a positive electrode, a negative electrode, a separator disposed between the positive electrode and the negative electrode, and a non-aqueous electrolyte, wherein lithium metal precipitates in the negative electrode during charging and dissolves during discharging, and the separator includes a substrate and a spacer, and the lithium secondary battery includes a pressure release mechanism that releases gas inside the battery case to the outside of the battery case when the pressure inside the battery case reaches a predetermined value P, and the predetermined value P is less than 3 MPa.
[0009] According to the present disclosure, the rate at which the internal pressure of the battery increases in the event of an internal short circuit or the like can be reduced.
[0010] The novel features of the present invention are set forth in the appended claims, but the present invention, both in terms of structure and content, together with other objects and features of the present invention, will be better understood from the following detailed description taken in conjunction with the drawings.
[0011] Fig. 2 is a longitudinal sectional view schematically showing an example of a lithium secondary battery according to an embodiment of the present disclosure; Fig. 3 is a sectional view schematically showing a main part of the lithium secondary battery shown in Fig. 1; Fig. 4 is a top view showing an example of a spacer pattern; Fig. 5 is a top view showing another example of a spacer pattern; Fig. 6 is a top view showing yet another example of a spacer pattern.
[0012] Hereinafter, embodiments according to the present disclosure will be described using examples, but the embodiments according to the present disclosure are not limited to the examples described below. In the following description, specific numerical values and materials may be exemplified, but other numerical values and other materials may be applied as long as the invention according to the present disclosure can be implemented. In this specification, the expression "numerical value A to numerical value B" includes numerical value A and numerical value B and can be read as "numerical value A or more and numerical value B or less." In the following description, when lower and upper limits are exemplified for numerical values of specific physical properties or conditions, any of the exemplified lower limits and any of the exemplified upper limits can be arbitrarily combined, as long as the lower limit is not equal to or greater than the upper limit.
[0013] (Lithium secondary battery) A lithium secondary battery according to an embodiment of the present disclosure includes a power generating element and a battery case that seals the power generating element. The power generating element includes a positive electrode, a negative electrode, a separator disposed between the positive electrode and the negative electrode, and a non-aqueous electrolyte. Lithium metal precipitates in the negative electrode during charging and dissolves during discharging. Specifically, the negative electrode includes at least a negative electrode current collector, and lithium metal precipitates on the negative electrode current collector. The non-aqueous electrolyte has lithium ion conductivity. Lithium secondary batteries are also called lithium metal secondary batteries.
[0014] In a lithium secondary battery, for example, 70% or more of the rated capacity is achieved by the deposition and dissolution of lithium metal. The movement of electrons at the negative electrode during charging and discharging is mainly due to the deposition and dissolution of lithium metal at the negative electrode. Specifically, 70 to 100% (e.g., 80 to 100% or 90 to 100%) of the movement of electrons (or current from another perspective) at the negative electrode during charging and discharging is due to the deposition and dissolution of lithium metal. In other words, the negative electrode of a lithium secondary battery differs from a negative electrode in which the movement of electrons at the negative electrode during charging and discharging is mainly due to the absorption and release of lithium ions by the negative electrode active material (e.g., graphite).
[0015] The positive electrode, negative electrode, and separator may be collectively referred to as an "electrode group." The positive electrode, negative electrode, and separator may be wound with a separator disposed between the positive electrode and the negative electrode to form a wound electrode group having multiple turns. When forming a wound electrode group, a strip-shaped positive electrode, a strip-shaped negative electrode, and a strip-shaped separator are usually used. The electrode group may be a laminate of a positive electrode, a separator, and a negative electrode.
[0016] The separator includes a substrate and a spacer. The lithium secondary battery includes a pressure release mechanism that releases gas from the battery case to the outside when the pressure inside the battery case reaches a predetermined value P. The predetermined value P is less than 3 MPa. Hereinafter, the predetermined value P will also be referred to as the operating pressure of the pressure release mechanism.
[0017] During charging, Li ions released from the positive electrode are reduced at the negative electrode and precipitate as metallic Li. As charging progresses, additional Li is deposited on top of the Li deposited at the beginning of charging. When the separator has a spacer, the spacer is non-conductive and presses against the negative electrode, suppressing Li deposition in the area of the negative electrode facing the spacer. On the other hand, Li deposition preferentially proceeds in the area of the negative electrode not facing the spacer. However, because the space formed between the positive and negative electrodes is limited by the spacer, Li deposits densely, resulting in a small surface area. This reduces the reaction area of the negative electrode, somewhat slowing the increase in the reaction rate of reactive gas generation associated with internal short circuits, etc. When the operating pressure of the pressure release mechanism is less than 3 MPa, the internal pressure of the battery is released and gas and heat are exhausted at a stage when the reaction rate is increasing slowly, significantly reducing the rate of increase in internal battery pressure. Note that an increase in internal battery pressure due to gas generation can be caused by, for example, an internal short circuit, an external short circuit, overcharging, etc.
[0018] From the viewpoint of reducing the rate of increase in the battery internal pressure, the predetermined value P is preferably 2.5 MPa or less. From the viewpoint of ensuring the reliability of the operation of the pressure release mechanism, the predetermined value P may be 0.8 MPa or more. The predetermined value P can be measured by a known method. As an example, the predetermined value P can be measured by clamping and fixing the outer periphery of the pressure release mechanism (for example, a metal plate having a thin portion, as described below) with a jig, gradually pressurizing it with air pressure, and obtaining the pressure value when the pressure release mechanism operates (the maximum pressure value when pressurized). The gas used for pressurization may be air, nitrogen, or argon.
[0019] (Pressure Release Mechanism) The pressure release mechanism releases gas and releases pressure when the internal battery pressure reaches a predetermined value P due to gas generation caused by an internal short circuit or the like. For example, the battery case may be equipped with the pressure release mechanism (e.g., a pressure release valve). The battery case may include, for example, a case body that houses the power generating element and a sealing body that seals the opening of the case body. The case body is, for example, cylindrical with a bottom. The sealing body or the bottom of the case body may be equipped with the pressure release mechanism (e.g., a pressure release valve).
[0020] For example, the sealing body may include a metal plate having a thin-walled portion that breaks when the pressure inside the battery case reaches a predetermined value P, and the pressure release mechanism may be activated by the breakage of the thin-walled portion. The thin-walled portion functions as a pressure release valve. The metal plate may have at least a thin-walled portion, and the entire metal plate may be a thin-walled portion. For example, the sealing body 16 in FIG. 1 includes an upper valve body 25 as a metal plate whose entire portion is made up of a thin-walled portion.
[0021] From the viewpoint of releasing the pressure inside the battery and facilitating the discharge of gas and heat while the reaction rate is increasing slowly, the ratio of the thickness T (mm) of the thin-walled portion to the maximum diameter D (mm) of the sealing body (T / D) may be less than 0.009 or may be 0.007 or less. Furthermore, from the viewpoint of ensuring the hermeticity of the battery when the internal pressure of the battery increases due to gas generation during normal use (charging and discharging) of the battery, T / D may be 0.002 or more. In the case of sealing body 16 of FIG. 1 , the maximum diameter D is the diameter of disc-shaped upper valve body 25, and the thickness T of the thin-walled portion is the thickness of upper valve body 25.
[0022] A sealing body equipped with a pressure release mechanism, such as sealing body 16 in Fig. 1, may also be equipped with a mechanism that cuts off current when the battery's internal pressure reaches a predetermined value PA. By cutting off current at a stage when the increase in the reaction rate of gas generation due to a short circuit or the like is relatively gradual, the rate of increase in the battery's internal pressure can be further reduced. The operating pressure PA of the current cutoff mechanism is approximately the same as or lower than the operating pressure P of the pressure release mechanism.
[0023] (Separator) The separator includes a substrate and a spacer.
[0024] (Substrate) A porous sheet having ion permeability and insulating properties is used as the substrate. Examples of the porous sheet include a microporous thin film, a woven fabric, and a nonwoven fabric. The material of the porous sheet is not particularly limited, but may be a polymer material. Examples of the polymer material include an olefin resin, a polyamide resin, and cellulose. Examples of the olefin resin include polyethylene, polypropylene, and a copolymer of ethylene and propylene. The substrate may contain an additive, if necessary. Examples of the additive include an inorganic filler.
[0025] The thickness of the substrate is not particularly limited, but is, for example, 5 μm or more and 20 μm or less, and more preferably 10 μm or more and 20 μm or less.
[0026] The substrate may include a porous sheet and a composite material layer (heat-resistant layer). The composite material layer may be formed on one or both main surfaces of the porous sheet. The composite material layer is a layer that allows lithium ions to permeate. The composite material layer contains inorganic particles. The composite material layer may contain a resin material as needed. The thickness of the composite material layer may be 5% to 50% of the total thickness of the substrate.
[0027] The composite material layer may be disposed on the side of the porous sheet facing the positive electrode, or on the side of the porous sheet facing the negative electrode. When the composite material layer is disposed on the positive electrode side, deterioration of the porous sheet due to oxidation reactions can be suppressed. When the composite material layer is disposed on the negative electrode side, deterioration of the porous sheet due to reduction reactions can be suppressed. A spacer may be disposed on the composite material layer. In this case, the effect of suppressing thermal shrinkage of the substrate is particularly enhanced.
[0028] The inorganic particles are preferably particles of an inorganic compound that is thermally stable and insulating, and thus unlikely to melt or decompose during abnormal heat generation due to a short circuit in the battery, etc. Examples of inorganic particle materials include oxides, hydroxides, nitrides, carbides, sulfides, etc. Examples of oxides include aluminum oxide, boehmite, magnesium oxide, titanium oxide, zirconium oxide, silicon oxide, yttrium oxide, zinc oxide, etc. Examples of nitrides include silicon nitride, aluminum nitride, boron nitride, titanium nitride, etc. Examples of carbides include silicon carbide and boron carbide, etc. Examples of sulfides include barium sulfate, etc. Examples of hydroxides include aluminum hydroxide, etc. The median diameter in the volume-based particle size distribution of the inorganic particles may be 0.2 to 2.0 μm.
[0029] The median diameter in the volume-based particle size distribution of inorganic particles can be measured, for example, using a laser diffraction / scattering particle size distribution measuring device (for example, Microtrac manufactured by Nikkiso Co., Ltd.) Alternatively, the cross section of the substrate may be observed with a transmission electron microscope (TEM), a TEM image may be taken, the area surrounded by the outlines of any 100 inorganic particles may be calculated, the diameter of an equivalent circle (perfect circle) having the same area as the calculated area may be determined, and the average diameter of the 100 equivalent circles may be calculated.
[0030] Examples of resin materials contained in the composite material layer (heat-resistant layer) include fluorine-containing resins such as polyvinylidene fluoride (PVdF) and polytetrafluoroethylene, fluorine-containing rubbers such as vinylidene fluoride-tetrafluoroethylene copolymer and ethylene-tetrafluoroethylene copolymer, styrene-butadiene copolymer or hydrogenated product thereof, acrylonitrile-butadiene copolymer or hydrogenated product thereof, methacrylic acid ester-acrylic acid ester copolymer, styrene-acrylic acid ester copolymer, acrylonitrile-acrylic acid ester copolymer, ethylene propylene rubber, polyvinyl alcohol, and rubbers such as polyvinyl acetate. Examples of the resin include cellulose derivatives such as ethyl cellulose, methyl cellulose, hydroxyethyl cellulose, and carboxymethyl cellulose; acrylic resins such as acrylic acid-methacrylic acid copolymers; polyphenylene ether, polysulfone, polyether sulfone, polyphenylene sulfide, polyetherimide, polyimide, polyamides such as wholly aromatic polyamide (aramid); polyamideimide, polyacrylonitrile, polyvinyl alcohol, polyether, polyacrylic acid, polymethacrylic acid, polyester, polyolefin, silicone resin, urethane resin, melamine resin, urea resin, and epoxy resin.
[0031] The resin material contained in the composite material layer (heat-resistant layer) is preferably a polymeric material having higher heat resistance than the material of the porous sheet. Such a polymeric material preferably includes at least one selected from the group consisting of aromatic polyamides, aromatic polyimides, and aromatic polyamideimides. These are known to have high heat resistance. From the viewpoint of heat resistance, aramids, i.e., meta-aramids (meta-type wholly aromatic polyamides) and para-aramids (para-type wholly aromatic polyamides), are preferred.
[0032] The content of the inorganic particles in the composite material layer may be in the range of 50% by weight to 99% by weight (for example, in the range of 85% by weight to 99% by weight).
[0033] The composite material layer is formed, for example, by applying a coating liquid containing inorganic particles, a resin material, and a liquid component (dispersion medium) to a porous sheet and then drying the coating film. Examples of the liquid component include N-methyl-2-pyrrolidone.
[0034] (Spacer) The spacer is formed on the main surface of the substrate. The spacer may be provided on the main surface of the substrate facing the negative electrode, on the main surface of the substrate facing the positive electrode, or on both main surfaces. When the spacer is provided on the main surface of the substrate facing the positive electrode, Li precipitates between the spacers so as to stretch the substrate toward the positive electrode, compared to when the spacer is provided on the main surface of the substrate facing the negative electrode. This generates compressive stress in the precipitated Li, making it easier for Li to precipitate densely. From the viewpoint of improving discharge efficiency and cycle characteristics, the spacer is preferably provided on the main surface of the substrate facing the positive electrode. On the other hand, when the spacer is provided on the main surface of the substrate facing the negative electrode, a space is formed in advance between the substrate and the negative electrode, so the tensile load on the substrate caused by the precipitation of Li is reduced. In other words, this is advantageous in that it is easier to maintain the insulating properties of the separator or the short-circuit resistance of the separator. From the viewpoint of easily reducing the rate of increase in the internal pressure of the battery in the event of an internal short circuit, the spacer is preferably provided on the main surface of the substrate facing the negative electrode.
[0035] In lithium secondary batteries, the main role of the spacer is to form a space for lithium metal to deposit, which prevents the negative electrode from expanding during charging.
[0036] The spacer may include a resin material (e.g., an insulating resin) or may include a resin material and particles. The proportion of the resin material in the spacer may be 10% by volume or more, 30% by volume or more, or 50% by volume or more, or may be 100% by volume or less, or 80% by volume or less.
[0037] Examples of resin materials contained in the spacer include fluorine-containing resins such as polyvinylidene fluoride (PVdF) and polytetrafluoroethylene, fluorine-containing rubbers such as vinylidene fluoride-tetrafluoroethylene copolymer and ethylene-tetrafluoroethylene copolymer, styrene-butadiene copolymer or its hydrogenated product, acrylonitrile-butadiene copolymer or its hydrogenated product, methacrylic acid ester-acrylic acid ester copolymer, styrene-acrylic acid ester copolymer, acrylonitrile-acrylic acid ester copolymer, rubbers such as ethylene propylene rubber, polyvinyl alcohol, and polyvinyl acetate, Examples of the resin include cellulose derivatives such as ethyl cellulose, methyl cellulose, hydroxyethyl cellulose, and carboxymethyl cellulose; acrylic resins such as acrylic acid-methacrylic acid copolymers; polyphenylene ether, polysulfone, polyether sulfone, polyphenylene sulfide, polyetherimide, polyimide, polyamides such as wholly aromatic polyamide (aramid); polyamideimide, polyacrylonitrile, polyvinyl alcohol, polyether, polyacrylic acid, polymethacrylic acid, polyester, polyolefin, silicone resin, urethane resin, melamine resin, urea resin, and epoxy resin.
[0038] Among the above resin materials, polyimide, polyvinylidene fluoride, acrylonitrile-acrylic acid ester copolymer, etc. are preferred as materials that do not allow lithium ions to pass through, and polyimide may also be used. A non-porous spacer of a certain height or more formed from these resin materials is a layer that does not allow lithium ions to pass through. The placement of such a spacer is preferable from the viewpoint of suppressing an increase in the gas generation reaction rate during an internal short circuit.
[0039] The particles may be inorganic or organic. Examples of inorganic particles include insulating metal oxides, metal hydroxides, metal nitrides, metal carbides, and metal sulfides. Examples of metal oxides include aluminum oxide (alumina and boehmite), magnesium oxide, titanium oxide (titania), zirconium oxide, and silicon oxide (silica). Examples of metal hydroxides include aluminum hydroxide. Examples of metal nitrides include silicon nitride, aluminum nitride, boron nitride, and titanium nitride. Examples of metal carbides include silicon carbide and boron carbide. Examples of metal sulfides include barium sulfate. Minerals such as aluminosilicates, layered silicates, barium titanate, and strontium titanate may also be used. Among these, alumina, silica, and titania are preferred.
[0040] The average particle size of the particles is not particularly limited, but may be 0.1 μm or more, 0.5 μm or more, or 10 μm or less, 5 μm or less, or 2 μm or less. The average particle size can be measured by the following method. First, a cross-section of the spacer in the thickness direction of the separator is photographed using an electron microscope to obtain an image of the cross-section. Next, the image is subjected to image processing such as binarization to identify the particle portion. Next, the diameter of a circle having the same area as the cross-section area of each particle (equivalent circle diameter) is determined, and the arithmetic mean of the determined equivalent circle diameters can be used as the average particle size. The arithmetic mean can be determined, for example, from 100 or more particles. The average particle size of other particles contained in the electrode plate and separator can also be determined by a similar method.
[0041] When the spacer contains a resin material and particles, the particle content in the spacer is preferably 50% by volume or less, which makes it easier to ensure sufficient strength of the spacer.
[0042] The area S1 of the spacer may be 30% or less of the area S0 of the substrate. This range ensures sufficient space for lithium metal deposition. The areas S1 and S0 are the areas of the substrate when viewed from the spacer side. The ratio of the area S1 to the area S0, S1 / S0, may be 0.20 or less (20% or less) or 0.10 or less, or may be 0.03 or more (3% or more) or 0.05 or more. From the viewpoint of suppressing an increase in the gas generation reaction rate during an internal short circuit, the S1 / S0 ratio is preferably 0.05 or more (5% or more).
[0043] The spacer preferably includes at least linear protrusions, and may be composed of only linear protrusions. From one perspective, the linear protrusions are ridge-shaped protrusions. The linear protrusions may be arranged intermittently, but from the viewpoint of suppressing an increase in the gas generation reaction rate during an internal short circuit, it is preferable that the linear protrusions are arranged continuously. The spacer may include dot-shaped protrusions.
[0044] The width of the linear convex portion may be 100 μm or more, or 200 μm or more, and may be 2000 μm or less, or 1000 μm or less.
[0045] The spacer preferably has a predetermined repeating pattern. That is, the convex portions are preferably arranged in a predetermined pattern. From the viewpoint of suppressing an increase in the gas generation reaction rate during an internal short circuit, it is particularly preferable that the linear convex portions are arranged in a mesh pattern. The mesh pattern may be an aggregate of polygons. An example of a mesh pattern includes a shape in which polygons are combined so as to share sides. Polygons include triangles, quadrilaterals, hexagons, etc. Different types of polygons may be combined. The mesh pattern may be honeycomb-shaped. Furthermore, the linear convex portions may be arranged in a striped pattern.
[0046] The height Hs of the spacer (protrusion) may be greater than the thickness Tw of the substrate. The ratio of the height Hs to the thickness Tw, Hs / Tw, may be greater than 1, 1.5 or greater, 2 or greater, or 3 or greater. Hs / Tw may be 10 or less, 8 or less, 5 or less, or 4 or less. By making Hs / Tw 1.5 or greater, expansion of the electrode group can be particularly suppressed.
[0047] The height Hs can be measured by the following method. First, a cross section of the separator (substrate) in the thickness direction is photographed using an electron microscope to obtain an image of the cross section. Next, 20 arbitrary locations among the spacers are selected in the image, and the heights of the spacers at those locations are measured. Next, the heights measured at the 20 locations are arithmetically averaged, and the obtained average value is defined as the height Hs. The thickness Tw can also be measured using a similar procedure.
[0048] The spacers are formed, for example, by applying a coating liquid containing spacer components and a liquid component to a predetermined location on a substrate and drying the coating. Examples of the liquid component include N-methyl-2-pyrrolidone. The coating may be performed using a dispenser or by a known printing method such as gravure printing, inkjet printing, or screen printing. The drying may be performed by a known method such as drying by heating or natural drying.
[0049] (Negative electrode) The negative electrode includes a negative electrode current collector. In a lithium secondary battery, lithium metal is deposited on the surface of the negative electrode upon charging. More specifically, lithium ions contained in the non-aqueous electrolyte receive electrons on the negative electrode upon charging, becoming lithium metal, which is then deposited on the surface of the negative electrode. The lithium metal deposited on the surface of the negative electrode dissolves as lithium ions in the non-aqueous electrolyte upon discharging.
[0050] The negative electrode may include a lithium ion occlusion layer (a layer that develops capacity by occlusion and release of lithium ions by a negative electrode active material (such as graphite)) supported on a negative electrode current collector. In this case, the open circuit potential of the negative electrode when fully charged may be 70 mV or less relative to lithium metal (dissolution and deposition potential of lithium). If the open circuit potential of the negative electrode when fully charged is 70 mV or less relative to lithium metal, lithium metal is present on the surface of the lithium ion occlusion layer when fully charged. In other words, the negative electrode develops capacity by deposition and dissolution of lithium metal.
[0051] Here, "fully charged" refers to a state in which the battery is charged to a state of charge of, for example, 0.98 x C or more, where C is the rated capacity of the battery. The open circuit potential of the negative electrode at full charge can be measured by disassembling a fully charged battery under an argon atmosphere, removing the negative electrode, and assembling a cell with lithium metal as the counter electrode. The nonaqueous electrolyte of the cell may have the same composition as the nonaqueous electrolyte in the disassembled battery.
[0052] The lithium ion occlusion layer is a layer of a negative electrode mixture containing a negative electrode active material. The negative electrode mixture may contain a binder, a thickener, a conductive agent, etc. in addition to the negative electrode active material.
[0053] Examples of the negative electrode active material include a carbonaceous material, a Si-containing material, and a Sn-containing material. The negative electrode may contain one or more negative electrode active materials. Examples of the carbonaceous material include graphite, easily graphitizable carbon (soft carbon), and hardly graphitizable carbon (hard carbon).
[0054] The conductive material is, for example, a carbon material, such as carbon black, acetylene black, ketjen black, carbon nanotubes, and graphite.
[0055] Examples of the binder include fluororesin, polyacrylonitrile, polyimide resin, acrylic resin, polyolefin resin, rubber polymer, etc. Examples of the fluororesin include polytetrafluoroethylene, polyvinylidene fluoride, etc.
[0056] The negative electrode current collector may be a conductive sheet, such as a foil or film.
[0057] The material of the negative electrode current collector (conductive sheet) may be any conductive material other than lithium metal and lithium alloys. The conductive material may be a metallic material such as a metal or alloy. The conductive material is preferably a material that does not react with lithium. More specifically, a material that does not form an alloy or an intermetallic compound with lithium is preferred. Examples of such conductive materials include copper (Cu), nickel (Ni), iron (Fe), and alloys containing these metal elements, as well as graphite with a preferentially exposed basal plane. Examples of alloys include copper alloys and stainless steel (SUS). Among these, copper and / or copper alloys with high conductivity are preferred.
[0058] The thickness of the negative electrode current collector is not particularly limited and is, for example, 5 μm or more and 300 μm or less.
[0059] (Positive Electrode) The positive electrode includes, for example, a positive electrode current collector and a positive electrode mixture layer supported on the positive electrode current collector. The positive electrode mixture layer includes, for example, a positive electrode active material, a conductive material, and a binder. The positive electrode mixture layer may be formed on only one side of the positive electrode current collector, or may be formed on both sides. The positive electrode is obtained, for example, by applying a positive electrode mixture slurry including the positive electrode active material, the conductive material, and the binder to both sides of the positive electrode current collector, drying the coating, and then rolling.
[0060] The positive electrode active material is a material that absorbs and releases lithium ions. Examples of the positive electrode active material include lithium-containing transition metal oxides, transition metal fluorides, polyanions, fluorinated polyanions, and transition metal sulfides. Among these, lithium-containing transition metal oxides are preferred because of their low production cost and high average discharge voltage.
[0061] The lithium contained in the lithium-containing transition metal oxide is released from the positive electrode as lithium ions during charging and precipitates as lithium metal on the negative electrode or negative electrode current collector. During discharging, the lithium metal dissolves from the negative electrode, releasing lithium ions, which are then absorbed into the composite oxide of the positive electrode. In other words, the lithium ions involved in charging and discharging are generally derived from the solute in the nonaqueous electrolyte and the positive electrode active material.
[0062] Examples of transition metal elements contained in the lithium-containing transition metal oxide include Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Y, Zr, and W. The lithium-containing transition metal oxide may contain one or more transition metal elements. The transition metal element may be Ni, Co, and / or Mn. The lithium-containing transition metal oxide may contain one or more typical elements as needed. Examples of typical elements include Mg, Al, Ca, Zn, Ga, Ge, Sn, Sb, Pb, and Bi. The typical element may be Al, etc.
[0063] Among lithium-containing transition metal oxides, composite oxides containing Ni, Co, and / or Mn as transition metal elements, and which may contain Al as an optional component, and which have a layered rock-salt crystal structure are preferred in terms of obtaining high capacity. In this case, in the lithium secondary battery, the molar ratio mLi / mM of the total amount of lithium contained in the positive electrode and negative electrode to the amount mM of metal M other than lithium contained in the positive electrode is set to, for example, 1.1 or less.
[0064] As the binder, conductive agent, etc., for example, those exemplified for the negative electrode can be used. The shape and thickness of the positive electrode current collector can be selected from the shape and range of the positive electrode current collector.
[0065] Examples of the material of the positive electrode current collector (conductive sheet) include metal materials containing Al, Ti, Fe, etc. The metal material may be Al, an Al alloy, Ti, a Ti alloy, an Fe alloy, etc. The Fe alloy may be stainless steel (SUS).
[0066] The thickness of the positive electrode current collector is not particularly limited and is, for example, 5 μm or more and 300 μm or less.
[0067] (Non-aqueous electrolyte) The non-aqueous electrolyte having lithium ion conductivity may be a liquid electrolyte (electrolytic solution), a gel electrolyte, or a solid electrolyte. The liquid electrolyte is, for example, an electrolytic solution containing a non-aqueous solvent and a lithium salt dissolved in the non-aqueous solvent. The concentration of the lithium salt in the electrolytic solution is, for example, 0.5 mol / L or more and 2 mol / L or less. The electrolytic solution may contain known additives.
[0068] The gel electrolyte contains a lithium salt and a matrix polymer, or a lithium salt, a non-aqueous solvent, and a matrix polymer. The matrix polymer is, for example, a polymer material that absorbs the non-aqueous solvent and gels. Examples of the polymer material include fluororesin, acrylic resin, polyether resin, and polyethylene oxide.
[0069] As the solid electrolyte, for example, a material known in all-solid-state lithium ion secondary batteries (for example, oxide-based solid electrolytes, sulfide-based solid electrolytes, halide-based solid electrolytes, etc.) can be used.
[0070] The liquid non-aqueous electrolyte is prepared by dissolving a lithium salt in a non-aqueous solvent, which generates lithium ions and anions.
[0071] The anion is BF 4 - , ClO 4 - , P.F. 6 - , C.F. 3 SO 3 - , C.F. 3 CO 2 - , anions of imides, anions of oxalate complexes, etc. Examples of the anions of imides include N(SO 2 CF 3 ) 2 - , N(C m F 2m+1 SO 2 ) x (C n F 2n+1 SO 2 )y - (m and n are each independently an integer of 0 or 1 or more, and x and y are each independently 0, 1, or 2, satisfying the relationship x+y=2). The anion of the oxalate complex may contain boron and / or phosphorus. Examples of the anion of the oxalate complex include bisoxalate borate anion and difluorooxalate borate anion (BF 2 (C 2 O 4 ) - ), P.F. 4 (C 2 O 4 ) - , P.F. 2 (C 2 O 4 ) 2 - The non-aqueous electrolyte may contain one of these anions alone or two or more of them.
[0072] From the viewpoint of suppressing the deposition of lithium metal in a dendritic form, the nonaqueous electrolyte preferably contains at least an anion of an oxalate complex, and more preferably contains an oxalate complex anion having fluorine. The interaction between the oxalate complex anion having fluorine and lithium facilitates the uniform deposition of lithium metal in the form of fine particles. This makes it easier to suppress local deposition of lithium metal. The oxalate complex anion having fluorine may be combined with another anion. The other anion may be PF 6 - and / or an anion of an imide.
[0073] Examples of non-aqueous solvents include esters, ethers, nitriles, amides, and halogen-substituted derivatives thereof. The non-aqueous electrolyte may contain one or more of these non-aqueous solvents. Examples of halogen-substituted derivatives include fluorides.
[0074] Examples of esters include carbonate esters and carboxylic acid esters. Examples of cyclic carbonate esters include ethylene carbonate, propylene carbonate, and fluoroethylene carbonate (FEC). Examples of chain carbonate esters include dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), and diethyl carbonate. Examples of cyclic carboxylic acid esters include γ-butyrolactone and γ-valerolactone. Examples of chain carboxylic acid esters include ethyl acetate, methyl propionate, and methyl fluoropropionate.
[0075] Examples of the ether include cyclic ethers and chain ethers. Examples of the cyclic ethers include 1,3-dioxolane, 4-methyl-1,3-dioxolane, tetrahydrofuran, and 2-methyltetrahydrofuran. Examples of the chain ethers include 1,2-dimethoxyethane, diethyl ether, ethyl vinyl ether, methyl phenyl ether, benzyl ethyl ether, diphenyl ether, dibenzyl ether, 1,2-diethoxyethane, and diethylene glycol dimethyl ether.
[0076] The concentration of the lithium salt in the non-aqueous electrolyte is, for example, 0.5 mol / L or more and 3.5 mol / L or less. The concentration of the anion in the non-aqueous electrolyte may be 0.5 mol / L or more and 3.5 mol / L or less. Furthermore, the concentration of the anion of the oxalate complex in the non-aqueous electrolyte may be 0.05 mol / L or more and 1 mol / L or less.
[0077] The non-aqueous electrolyte may contain an additive. The additive may form a coating on the negative electrode. The formation of a coating derived from the additive on the negative electrode makes it easier to suppress the formation of dendrites. Examples of such additives include vinylene carbonate, FEC, and vinyl ethyl carbonate (VEC).
[0078] From the viewpoint of thermal stability, fluorine atom-containing cyclic carbonate esters are preferred, and FEC is more preferred. When the nonaqueous solvent is an ether-based solvent containing an ether, the amount of gas generated upon internal short circuit is greater than when the nonaqueous solvent contains fluorine atom-containing cyclic carbonate esters (e.g., FEC), and therefore the effect of reducing the rate of increase in the internal pressure of the battery according to the present disclosure can be significantly achieved.
[0079] An example of a lithium secondary battery according to the present embodiment will be described in detail below with reference to the drawings. The components described above can be applied to the components of the lithium secondary battery of the example described below. The components of the example described below can be modified based on the above description. The matters described below may also be applied to the above embodiment. In the lithium secondary battery described below, components that are not essential for the lithium secondary battery according to the present disclosure may be omitted. Note that the scale of the components has been changed in the following drawings to facilitate understanding.
[0080] (Embodiment 1) FIG. 1 is a longitudinal cross-sectional view schematically illustrating an example of a lithium secondary battery according to Embodiment 1. Note that FIG. 1 does not illustrate spacers and spaces formed by the spacers. The cylindrical lithium secondary battery 10 shown in FIG. 1 includes a cylindrical battery case and a wound electrode group 14 and a nonaqueous electrolyte (not shown) housed within the battery case. The battery case includes a case body 15, which is a cylindrical metal container with a bottom, and a sealing member 16 that seals the opening of the case body 15. A gasket 27 is disposed between the case body 15 and the sealing member 16. The gasket 27 ensures the hermeticity of the battery case. Within the case body 15, insulating plates 17 and 18 are disposed at both ends of the electrode group 14 in the direction of the winding axis.
[0081] Case body 15 has a step 21 formed, for example, by pressing a portion of the side wall of case body 15 from the outside. Step 21 may be formed in an annular shape along the circumferential direction of case body 15 on the side wall of case body 15. In this case, sealing body 16 is supported by the surface of step 21 on the opening side.
[0082] The sealing body 16 includes a filter 22, a lower valve body 23, an insulating member 24, an upper valve body 25, and a cap 26. These components are stacked in this order in the sealing body 16. The sealing body 16 is attached to the opening of the case body 15 so that the cap 26 is located outside the case body 15 and the filter 22 is located inside the case body 15. The above-mentioned components constituting the sealing body 16 are, for example, disk-shaped or ring-shaped. The lower valve body 23 and the upper valve body 25 are connected to each other at their respective centers, and an insulating member 24 is interposed between their respective peripheral edges. The filter 22 and the lower valve body 23 are connected to each other at their respective centers. The upper valve body 25 and the cap 26 are connected to each other at their respective centers. In other words, all components except the insulating member 24 are electrically connected to each other.
[0083] The sealing body 16 of the first embodiment is equipped with a current interruption mechanism and a pressure release mechanism. The lower valve body 23 has a vent hole (not shown). Therefore, when the internal pressure of the battery case increases due to a short circuit (abnormal heat generation) or the like and reaches a predetermined value PA, the upper valve body 25 expands toward the cap 26 and separates from the lower valve body 23. This interrupts the electrical connection between the lower valve body 23 and the upper valve body 25. When the internal pressure further increases and reaches a predetermined value P, the upper valve body 25 breaks, and gas is released from an opening (not shown) formed in the cap 26. In the case of the sealing body 16, the operating pressure P of the pressure release mechanism is greater than the operating pressure PA of the electrical interruption mechanism.
[0084] 2 is an enlarged view of a portion of the electrode group 14. FIG. 2 includes a portion near the positive electrode surrounded by region II in FIG. 1 and a portion near the negative electrode surrounded by region III in FIG.
[0085] The electrode group 14 includes a positive electrode 11, a negative electrode 12, and a separator (a substrate 50 and a spacer 53). The positive electrode 11, the negative electrode 12, and the separator substrate 50 are all strip-shaped. The electrode group 14 is formed by winding the positive electrode 11, the negative electrode 12, and the separator (substrate 50) so that the separator is disposed between the positive electrode 11 and the negative electrode 12.
[0086] The positive electrode 11 includes a positive electrode current collector 11a and a positive electrode composite layer 11b. The positive electrode current collector 11a is electrically connected to a cap 26, which functions as a positive electrode terminal, via a positive electrode lead 19. In FIG. 2, the negative electrode 12 is shown as a negative electrode (negative electrode current collector) on which no lithium metal is deposited. The negative electrode 12 is electrically connected to a case body 15, which functions as a negative electrode terminal, via a negative electrode lead 20.
[0087] The substrate 50 has a first main surface 50a facing the negative electrode 12 and a second main surface 50b facing the positive electrode 11. The substrate 50 of embodiment 1 includes a porous sheet 51 and a composite material layer 52 (heat-resistant layer). The composite material layer 52 is formed on one of the two main surfaces of the porous sheet 51, the main surface facing the negative electrode 12. In embodiment 1, a spacer 53 is formed on the first main surface 50a. The spacer 53 is formed on the composite material layer 52 and is in contact with the negative electrode 12. The spacer 53 forms a space 14s between the positive electrode 11 and the negative electrode 12 (between the negative electrode 12 and the substrate 50). FIG. 2 shows the height h of the spacer 53.
[0088] In Fig. 2, the composite material layer 52 of the substrate 50 is disposed on the negative electrode 12 side, but it may be disposed on the positive electrode 11 side. The spacer 53 is formed on the composite material layer 52, but it may be formed on the porous sheet 51. The spacer 53 is disposed on the negative electrode 12 side of the substrate 50, but it may be disposed on the positive electrode 11 side of the substrate 50.
[0089] During charging of the lithium secondary battery 10, lithium metal is deposited on the negative electrode 12. Because a space 14s exists between the positive electrode 11 and the negative electrode 12, the volume change of the electrode group 14 that accompanies the deposition of lithium metal is reduced, improving the cycle characteristics.
[0090] An example of the planar shape of the spacer 53 is shown in Fig. 3. The spacer 53 in Fig. 3 is composed of linear protrusions 53a arranged in a honeycomb pattern. The linear protrusions 53a are arranged continuously. Areas where the spacers 53 are not formed form spaces 14s.
[0091] Other examples of the planar shape of the spacer 53 are shown in Figures 4 and 5. In the spacer 53 of Figure 4, linear protrusions 53a arranged in a honeycomb pattern have defects 53b, and the linear protrusions 53a are arranged intermittently. In the spacer 53 of Figure 5, multiple linear protrusions 53a are arranged in a stripe pattern. In Figure 5, six linear protrusions 53a are arranged, but the number of linear protrusions 53a is not limited to this. The linear protrusions 53a of Figure 5 are arranged along the length direction of the band-shaped substrate 50.
[0092] In the first embodiment, a cylindrical lithium secondary battery having a wound electrode group has been described. However, the lithium secondary battery of this embodiment is not limited to the form of the first embodiment, and can be applied to other forms. The shape of the lithium secondary battery can be appropriately selected from various shapes such as a cylindrical shape, a coin shape, a rectangular shape, a sheet shape, and a flat shape depending on the application. The shape of the electrode group is also not particularly limited, and may be a stacked type.
[0093] (Additional Notes) The above embodiments disclose the following technologies. (Technology 1) A lithium secondary battery comprising a power generating element and a battery case sealing the power generating element, wherein the power generating element comprises a positive electrode, a negative electrode, a separator disposed between the positive electrode and the negative electrode, and a non-aqueous electrolyte, wherein lithium metal precipitates in the negative electrode during charging and dissolves during discharging, and the separator has a substrate and a spacer, and the lithium secondary battery comprises a pressure release mechanism that releases gas inside the battery case to the outside of the battery case when the pressure inside the battery case reaches a predetermined value P, wherein the predetermined value P is less than 3 MPa. (Technology 2) The lithium secondary battery according to Technology 1, wherein the predetermined value P is 2.5 MPa or less. (Technology 3) The lithium secondary battery according to Technology 1 or 2, wherein the battery case comprises a cylindrical case body with a bottom that houses the power generating element and a sealing body that seals the opening of the case body, and wherein the sealing body or the bottom of the case body is provided with the pressure release mechanism. (Technology 4) The lithium secondary battery according to Technology 3, wherein the sealing body comprises a metal plate, and the metal plate has a thin-walled portion that breaks when the pressure inside the battery case reaches a predetermined value P, and the pressure release mechanism is activated by the breakage of the thin-walled portion. (Technology 5) The lithium secondary battery according to Technology 4, wherein the ratio T / D of the thickness T of the thin-walled portion to the maximum diameter D of the sealing body is less than 0.009. (Technology 6) The lithium secondary battery according to any one of Technology 1 to 5, wherein the spacer has a predetermined repeating pattern. (Technology 7) The lithium secondary battery according to any one of Technology 1 to 6, wherein the spacer includes a resin material. (Technology 8) The lithium secondary battery according to any one of Technologies 1 to 7, wherein the spacer is disposed on one main surface of the substrate. (Technology 9) The lithium secondary battery according to any one of Technologies 1 to 8, wherein the substrate comprises a porous sheet containing a polymer material and a composite material layer containing a resin material and inorganic particles. (Technology 10) The lithium secondary battery according to any one of Technologies 1 to 9, wherein the non-aqueous electrolyte contains an ether-based solvent.(Technology 11) The lithium secondary battery according to any one of Techniques 1 to 10, wherein the non-aqueous electrolyte contains an anion of an oxalate complex. (Technology 12) The lithium secondary battery according to Technique 11, wherein the anion of the oxalate complex contains a difluorooxalate borate anion.
[0094] [Examples] The lithium secondary battery according to the present disclosure will be described in more detail below based on examples and comparative examples, although the present disclosure is not limited to the following examples.
[0095] Example 1 (Preparation of Positive Electrode) A positive electrode active material, acetylene black (AB; conductive material), polyvinylidene fluoride (PVdF; binder), and an appropriate amount of N-methyl-2-pyrrolidone (NMP) were mixed to prepare a positive electrode mixture slurry. The positive electrode active material was a rock-salt lithium-containing transition metal oxide (NCA; positive electrode active material) containing Li, Ni, Co, and Al (the molar ratio of Li to the total of Ni, Co, and Al was 1.0) and having a layered structure. The mass ratio of NCA:AB:PVdF in the positive electrode mixture slurry was 95:2.5:2.5. The positive electrode mixture slurry was applied to both sides of a strip-shaped Al foil (positive electrode current collector), and the coating was dried and rolled to form a positive electrode mixture layer. The positive electrode current collector having the positive electrode mixture layers formed on both sides was cut to a predetermined size to obtain a positive electrode.
[0096] (Preparation of Negative Electrode Current Collector) A strip of electrolytic copper foil (thickness: 12 μm) was prepared as a negative electrode current collector.
[0097] (Preparation of Substrate) A 10 μm-thick polyethylene microporous thin film was prepared. One main surface of the microporous thin film was coated with a coating liquid containing paraphenylene terephthalamide, an aromatic polyamide, as the resin material and alumina as inorganic particles. The coating liquid was an N-methyl-2-pyrrolidone solution containing 5.8% by mass of dissolved calcium chloride, and the concentration was adjusted to 2 wt% of aromatic polyamide and 4 wt% of alumina. The substrate with the coating film formed was left for 1 hour in an atmosphere at 25°C and 70% relative humidity to precipitate the aromatic polyamide. Next, the NMP and calcium chloride in the coating film were removed by water washing. The coating film was dried at 60°C for 5 minutes to form a composite material layer (heat-resistant layer). In this manner, a substrate comprising a microporous thin film and a composite material layer was obtained.
[0098] (Formation of Spacers on the Main Surface of the Substrate) A coating solution containing polyvinylidene fluoride and alumina particles (inorganic filler) was applied to the microporous thin film surface of the substrate, and the coating was dried to form spacers in the pattern (honeycomb shape) shown in Figure 3. In this way, a separator having a substrate and spacers was obtained. The linear convex portions constituting the spacers had a width of 0.25 mm and a height of 30 μm. The area S1 of the spacers was 21% of the area S0 of the substrate.
[0099] (Preparation of non-aqueous electrolyte) 1,2-dimethoxyethane (DME) and 1,1,2,2-tetrafluoroethyl 2,2,2-trifluoroethyl ether (CHF 2 (CF 2 OCH 2 )CF 3 An ether-based mixed solvent containing lithium bis(sulfonylimide) (LiFSI) at 1 mol / L and LiBF at a volume ratio of 1:2 was prepared. 2 (C 2 O 4 ) was dissolved in the ethanol to a concentration of 0.1 mol / L to prepare a liquid non-aqueous electrolyte (ether-based electrolyte solution).
[0100] (Battery Assembly) In an inert gas atmosphere, a positive electrode and a negative electrode current collector were spirally wound with a separator interposed therebetween to prepare an electrode assembly. The separator was positioned so that the spacer faced the negative electrode. In this way, a wound electrode assembly having the structure shown in Figure 2 was obtained. The electrode assembly was housed in a cylindrical case body with a bottom, and a nonaqueous electrolyte was poured into it.
[0101] A sealing body (sealing body 16 in FIG. 1 ) equipped with a pressure release mechanism was prepared. The operating pressure P of the pressure release mechanism was set to 1.6 MPa by adjusting the thickness of the thin-walled portion of the metal plate of the sealing body (upper valve body 25 in FIG. 1 ). T / D, calculated from the diameter of upper valve body 25 (the maximum diameter D of the sealing body) and the thickness of upper valve body 25 (the thickness T of the thin-walled portion), was 0.004.
[0102] A sealing member was placed over the opening of the case body via a gasket, sealing the electrode group and non-aqueous electrolyte within the battery case, thus completing a lithium secondary battery A1 having the structure shown in FIG.
[0103] Example 2 A lithium secondary battery A2 was produced in the same manner as in Example 1, except that in producing the electrode group, the separator was arranged so that the spacer faced the positive electrode.
[0104] Example 3 A lithium secondary battery A3 was fabricated in the same manner as in Example 1, except that spacers having the pattern shown in Figure 4 were formed using a dispenser. The linear protrusions were arranged intermittently. The area S1 of the spacer was 17% of the area S0 of the substrate.
[0105] Example 4 A mixed solvent containing fluoroethylene carbonate (FEC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) in a volume ratio of 20:5:75 was prepared. 6 1 mol / L, LiBF 2 (C 2 O 4 ) were dissolved in the electrolyte at a concentration of 0.5 mol / L to prepare a liquid nonaqueous electrolyte (FEC-based electrolyte solution). A lithium secondary battery A4 was fabricated in the same manner as in Example 1 except for the above.
[0106] Examples 5 and 6 Lithium secondary batteries A5 and A6 were fabricated in the same manner as in Example 1, except that the operating pressure P of the pressure release mechanism was set to 1.9 MPa or 2.5 MPa by adjusting the thickness of the thin portion of the metal plate of the sealing body (upper valve body 25 in FIG. 1 ). The T / D was 0.005 (A5) or 0.007 (A6).
[0107] Example 7 A lithium secondary battery A7 was fabricated in the same manner as in Example 1, except that a spacer having the pattern shown in Fig. 5 was formed using a dispenser. The number of linear protrusions arranged in a stripe pattern was 26, and the width of the linear protrusions was 0.25 mm. The area S1 of the spacer was 20% of the area S0 of the substrate.
[0108] Comparative Example 1 A lithium secondary battery B1 was fabricated in the same manner as in Example 1, except that spacers in the pattern shown in Figure 5 were formed on both main surfaces of an electrolytic copper foil (negative electrode current collector) instead of forming spacers on one main surface of the substrate. The number of linear protrusions arranged in a stripe pattern was 26, and the width of the linear protrusions was 0.25 mm. The area S1 of the spacers was 20% of the area S0 of the substrate.
[0109] Comparative Example 2 A lithium secondary battery B2 was fabricated in the same manner as in Comparative Example 1, except that the same FEC-based electrolyte solution as in Example 4 was used as the non-aqueous electrolyte solution.
[0110] Comparative Example 3 A lithium secondary battery B3 was fabricated in the same manner as in Example 1, except that the operating pressure P of the pressure release mechanism was set to 3.0 MPa by adjusting the thickness of the thin portion of the metal plate of the sealing body (upper valve body 25 in FIG. 1 ). The T / D ratio was 0.009.
[0111] [Evaluation: Internal Short Circuit Test] Each of the obtained batteries was subjected to constant current charging at a current of 0.5 mA per unit area (cm 2 ) of the electrode until the battery voltage reached 4.2 V, and then constant voltage charging at a voltage of 4.2 V until the current value per unit area of the electrode reached 0.05 mA. In this way, a fully charged battery was obtained.
[0112] A fully charged battery was placed in a sealed container, and the battery was internally short-circuited and heated by a nail. An N45 nail (body diameter 2.45 mm) was used, and the nail penetration speed was 0.1 mm / sec. The internal short-circuit caused the battery to heat up, generating gas within the battery. The pressure release mechanism was activated, releasing the gas outside the battery. The pressure change over time within the sealed container was measured using a pressure sensor, and the amount of pressure change per unit time was calculated as the internal pressure differential (MPa / s). The maximum value of the internal pressure differential was calculated. Since the rate of gas release outside the battery depends on the gas generation rate inside the battery (rate of increase in internal battery pressure), the maximum value of the internal pressure differential was used as an indicator of the rate of increase in internal battery pressure.
[0113] The evaluation results are shown in Table 1. In Table 1, ○ indicates that the internal pressure differential value was 1 MPa / s or less, and the rate of internal pressure rise was significantly reduced. △ indicates that the internal pressure differential value was more than 1 MPa / s and less than 4 MPa / s, and the rate of internal pressure rise was kept relatively low. × indicates that the internal pressure differential value was 4 MPa / s or more, and the rate of internal pressure rise was significantly increased.
[0114]
[0115] In the batteries A1 to A7, in which a spacer was formed on one side of the separator substrate and the operating pressure of the pressure release mechanism was set to less than 3.0 MPa, the rate of increase in internal pressure was reduced.
[0116] In batteries B1 and B2, the operating pressure of the pressure release mechanism was set to less than 3.0 MPa, but spacers were formed on both sides of the negative electrode current collector, which significantly increased the rate of internal pressure increase during an internal short circuit.In battery B3, a spacer was formed on one side of the separator substrate, but the operating pressure of the pressure release mechanism was set to 3.0 MPa, which significantly increased the rate of internal pressure increase.
[0117] The lithium secondary battery of the present disclosure can be used in electronic devices such as mobile phones, smartphones, and tablet terminals, electric vehicles including hybrids and plug-in hybrids, and home storage batteries combined with solar cells.
[0118] While the present invention has been described in terms of presently preferred embodiments, such disclosure is not to be interpreted as limiting. Various changes and modifications will no doubt become apparent to those skilled in the art to which the present invention pertains upon reading the above disclosure. It is therefore intended that the appended claims be interpreted to cover all changes and modifications that do not depart from the true spirit and scope of the invention.
[0119] REFERENCE SIGNS LIST 10: Lithium secondary battery 11: Positive electrode 12: Negative electrode 14: Electrode group 14s: Space 15: Case body 16: Sealing body 23: Lower valve body 25: Upper valve body 50: Substrate 51: Porous sheet 52: Composite material layer 53: Spacer 53a: Convex portion
Claims
1. A lithium secondary battery comprising a power generating element and a battery case sealing the power generating element, wherein the power generating element comprises a positive electrode, a negative electrode, a separator disposed between the positive electrode and the negative electrode, and a non-aqueous electrolyte, wherein lithium metal precipitates in the negative electrode during charging and dissolves during discharging, the separator has a substrate and a spacer, and wherein the lithium secondary battery comprises a pressure release mechanism that releases gas within the battery case to the outside of the battery case when the pressure within the battery case reaches a predetermined value P, and wherein the predetermined value P is less than 3 MPa.
2. The lithium secondary battery according to claim 1, wherein the predetermined value P is 2.5 MPa or less.
3. The lithium secondary battery described in claim 1, wherein the battery case comprises a bottomed cylindrical case body that houses the power generating element and a sealing body that seals an opening of the case body, and the sealing body or the bottom of the case body is provided with the pressure release mechanism.
4. The lithium secondary battery described in claim 3, wherein the sealing body comprises a metal plate, the metal plate having a thin-walled portion that breaks when the pressure inside the battery case reaches a predetermined value P, and the pressure release mechanism is activated by the breakage of the thin-walled portion.
5. The lithium secondary battery according to claim 4, wherein the ratio of the thickness T of said thin portion to the maximum diameter D of said sealing body: T / D is less than 0.
009.
6. The lithium secondary battery according to claim 1, wherein the spacers have a predetermined repeating pattern.
7. The lithium secondary battery according to claim 1, wherein the spacer includes a resin material.
8. The lithium secondary battery according to claim 1, wherein the spacer is disposed on one of the main surfaces of the substrate.
9. The lithium secondary battery according to claim 1, wherein the substrate comprises a porous sheet including a polymeric material and a composite material layer including a resin material and inorganic particles.
10. The lithium secondary battery according to claim 1, wherein the non-aqueous electrolyte contains an ether-based solvent.
11. The lithium secondary battery according to claim 1, wherein the non-aqueous electrolyte contains an anion of an oxalate complex.
12. The lithium secondary battery according to claim 11, wherein the anion of the oxalate complex comprises a difluorooxalatoborate anion.
Citation Information
Patent Citations
Lithium secondary battery
JP2019160776A
Sealed battery
JP2022031997A
Laminate for nonaqueous secondary batteries, method for producing same, wound body for nonaqueous secondary batteries, and method for producing nonaqueous secondary battery member
WO2019039357A1
Lithium secondary battery
WO2022045127A1
Lithium secondary battery
WO2023008460A1