Coloring agent, coloring composition, and method for producing coloring agent
Patent Information
- Application Number
- PCT/JP2024/012771
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-03
Smart Images

Figure JP2024012771_03102024_PF_FP_ABST
Abstract
Description
Colorant, coloring composition, and method for producing colorant
[0001] The present invention relates to a colorant, a coloring composition, and a method for producing the colorant. More specifically, the present invention relates to a colorant capable of reproducing hues from red to magenta, a coloring composition such as a printing ink containing the colorant, and a method for producing the colorant.
[0002] Examples of colorants capable of reproducing hues from red to magenta include organic pigments such as soluble azo pigments, insoluble azo pigments, and quinacridone pigments. These organic pigments are used in a variety of applications, including plastic products, toners, paints, and printing inks.
[0003] Among the above organic pigments, soluble azo pigments have the advantages of vivid hue, high tinting strength, and low cost. However, soluble azo pigments have problems with fastness. Furthermore, in some applications, the presence of metal ions used in pigment lake formation can adversely affect various printing characteristics. Quinacridone pigments have superior properties in fastness and vividness compared to other pigments. However, quinacridone pigments have problems in that they are significantly inferior in tinting strength or dispersion stability compared to other pigments, and are expensive.
[0004] On the other hand, naphthol-based azo pigments, which are classified as insoluble azo pigments, have been considered for use in various applications because they offer a good balance of production cost, coloring strength, and fastness. However, their clarity and dispersibility are insufficient, and improvements are desired. In addition, their crystal stability is low, and when combined with a dispersion medium, problems such as pigment crystal growth and increased particle size can occur.
[0005] In response to this, for example, in the field of digital printing, various studies have been conducted to improve naphthol-based azo pigments. For example, Patent Document 1 discloses a pigment composition containing a naphthol-based azo pigment and a specific azonaphthoic acid component, and a magenta color toner using the pigment composition. Furthermore, Patent Document 2 discloses a magenta toner containing a naphthol-based azo pigment, a binder resin, a colorant, and a wax component, and further containing a β-naphthol derivative and an aromatic amine in a specific ratio.
[0006] JP 2000-248191 A JP 2003-149869 A
[0007] However, the naphthol azo pigments disclosed in Patent Documents 1 and 2 are both colorants intended for toner applications, and when applied to paints or printing inks, there is room for improvement in terms of dispersibility. If the dispersibility of the pigment is insufficient, it becomes difficult to obtain desired properties in various applications.
[0008] For example, poor pigment dispersibility in aqueous dispersions such as aqueous inkjet inks or non-aqueous dispersions such as flexographic inks makes it difficult to achieve fully satisfactory coloring strength, vividness, and transparency. Furthermore, both aqueous and non-aqueous dispersions tend to suffer from problems such as increased viscosity during long-term storage. Therefore, there is a demand for colorants that have excellent pigment dispersibility, are applicable to various applications, and can provide desired properties.
[0009] Therefore, one embodiment of the present invention provides a naphthol azo pigment-based colorant that has excellent dispersibility and can improve coloring strength, vividness, and transparency. Another embodiment of the present invention also provides a coloring composition that uses the colorant and can be used for various applications such as printing inks. Furthermore, one embodiment of the present invention also provides a method for producing the colorant.
[0010] In view of the above-mentioned circumstances, the present inventors have investigated ways to improve the dispersibility of colorants based on naphthol azo pigments, and as a result have found that various properties can be improved by forming a colorant containing a naphthol azo pigment and a specific compound, which has led to the completion of the present invention.
[0011] That is, the present invention includes the following embodiments: However, the embodiments of the present invention are not limited to the following and include various embodiments.
[0012] One embodiment relates to a colorant containing a compound (A) represented by the following general formula (1) and a compound (B) represented by the following general formula (2).
[0013]
[0014]
[0015] In the general formula (1) and the general formula (2), R 1 ~R 5 and R 1 '~R 5 ' are each independently a hydrogen atom, an alkoxy group, an alkyl group, a halogen group, a nitro group, a carboxy group, a sulfo group, a phosphate group, a sulfamoyl group, a carbamoyl group, a benzamido group, an alkylsulfamoyl group, an alkylcarbamoyl group, a group represented by the following general formula (101), a group represented by the following general formula (102), or a group represented by the following chemical formula (103), and R 1 ~R 5 cannot all be hydrogen atoms at the same time, and R 1 '~R 5 ' cannot all be hydrogen atoms at the same time. 6 ~R 11 are each independently a hydrogen atom, an alkoxy group, an alkyl group, a halogen group, a nitro group, a carboxy group, a sulfo group, a phosphate group, a sulfamoyl group, a carbamoyl group, an alkylsulfamoyl group, an alkylcarbamoyl group, a group represented by the following general formula (104), or a group represented by the following general formula (105), and R 6 ~R 11 are not all hydrogen atoms at the same time. X is a hydrogen atom, a hydroxyl group, or a chlorine atom.
[0016]
[0017] In general formula (101), R 21 ~R 25 are each independently a hydrogen atom, an alkoxy group, an alkyl group, a halogen group, a nitro group, a carboxy group, a sulfo group, a phosphate group, a sulfamoyl group, a carbamoyl group, an alkylsulfamoyl group, an alkylcarbamoyl group, or an aryl group which may have a substituent, or R 21 ~R 25Two adjacent groups among these may combine together to form a saturated or unsaturated alkylene group, or a saturated or unsaturated heteroalkylene group containing one or more heteroatoms selected from the group consisting of oxygen atoms, nitrogen atoms, and sulfur atoms, or form a divalent group having a skeleton composed of a nitrogen atom and a carbonyl group, and the two adjacent groups may combine together with the carbon atoms to which they are bonded to form a ring.
[0018]
[0019] In general formula (102), R 26 ~R 30 are each independently a hydrogen atom, an alkoxy group, an alkyl group, a halogen group, a nitro group, a carboxy group, a sulfo group, a phosphate group, a sulfamoyl group, a carbamoyl group, an alkylsulfamoyl group, an alkylcarbamoyl group, or an aryl group which may have a substituent, or R 26 ~R 30 Two adjacent groups among these may combine together to form a saturated or unsaturated alkylene group, or a saturated or unsaturated heteroalkylene group containing one or more heteroatoms selected from the group consisting of oxygen atoms, nitrogen atoms, and sulfur atoms, or form a divalent group having a skeleton composed of a nitrogen atom and a carbonyl group, and the two adjacent groups may combine together with the carbon atoms to which they are bonded to form a ring.
[0020]
[0021]
[0022] In general formula (104), R 31 ~R 35 are each independently a hydrogen atom, an alkoxy group, an alkyl group, a halogen group, a nitro group, a carboxy group, a sulfo group, a phosphate group, a sulfamoyl group, a carbamoyl group, an alkylsulfamoyl group, an alkylcarbamoyl group, or an aryl group which may have a substituent, or R 31 ~R 35Two adjacent groups among these may combine together to form a saturated or unsaturated alkylene group, or a saturated or unsaturated heteroalkylene group containing one or more heteroatoms selected from the group consisting of oxygen atoms, nitrogen atoms, and sulfur atoms, or form a divalent group having a skeleton composed of a nitrogen atom and a carbonyl group, and the two adjacent groups may combine together with the carbon atoms to which they are bonded to form a ring.
[0023]
[0024] In general formula (105), R 36 ~R 40 are each independently a hydrogen atom, an alkoxy group, an alkyl group, a halogen group, a nitro group, a carboxy group, a sulfo group, a phosphate group, a sulfamoyl group, a carbamoyl group, an alkylsulfamoyl group, an alkylcarbamoyl group, or an aryl group which may have a substituent, or R 36 ~R 40 Two adjacent groups among these may combine together to form a saturated or unsaturated alkylene group, or a saturated or unsaturated heteroalkylene group containing one or more heteroatoms selected from the group consisting of oxygen atoms, nitrogen atoms, and sulfur atoms, or form a divalent group having a skeleton composed of a nitrogen atom and a carbonyl group, and the two adjacent groups may combine together with the carbon atoms to which they are bonded to form a ring.
[0025] In the above embodiment, the content of compound (B) relative to the total mass of compound (A) is preferably in the range of 0.01 to 10 mass%, more preferably 0.15 to 10 mass%.
[0026] One embodiment relates to a coloring composition including the colorant of the above embodiment and a dispersion medium. In one embodiment, the coloring composition may be a printing ink including a colorant, a resin, and a solvent. In another embodiment, the coloring composition may be an actinic ray-curable ink including a colorant and a polymerizable compound.
[0027] One embodiment relates to a method for producing a colorant containing a compound (A) represented by the above general formula (1) and a compound (B) represented by the above general formula (2), comprising carrying out a coupling reaction between a solution containing a coupler component represented by the following general formula (7) and a solution containing a diazonium salt represented by the following general formula (6A) obtained by diazotizing an aromatic amine, using an excess amount of diazonium salt in terms of molar ratio relative to the coupler component. 1 '~R 5 ' are R in the general formula (1) at the corresponding positions, respectively. 1 ~R 5 and have the same base.
[0028]
[0029] In general formula (7), R 6 ~R 11 is R in the above general formula (1). 6 ~R 11 is the same as:
[0030]
[0031] In general formula (6A), R 1 ~R 5 is R in the above general formula (1). 1 ~R 5 In one embodiment, the coupling reaction using the solution containing the coupler component and the solution containing the diazonium salt is preferably carried out in the presence of a water-soluble organic solvent. The disclosure of the present application is related to the subject matter described in Japanese Patent Application No. 2023-054361, filed on March 29, 2023, the entire disclosure of which is incorporated herein by reference.
[0032] According to an embodiment of the present invention, a colorant having excellent dispersibility and capable of improving coloring power, vividness, and transparency can be provided. In addition, a colored composition using the colorant that can be used for various applications can be provided.
[0033] Hereinafter, the embodiments of the present invention will be described in more detail. However, the present invention is not limited to the following embodiments, and various modifications may be made within the scope of the present invention, and various embodiments are included.
[0034] <1> Colorant One embodiment of the present invention relates to a colorant containing a compound (A) represented by the following general formula (1) and a compound (B) represented by the following general formula (2).
[0035] <Compound (A)> In the colorant of the above embodiment, compound (A) is a naphthol-based azo pigment having a structure represented by the following general formula (1). In the colorant, as compound (A), one of the naphthol-based azo pigments may be used alone, or two or more may be used in combination. In one embodiment, from the viewpoint of facilitating adjustment of color tone, compound (A) constituting the colorant preferably contains two or more naphthol-based azo pigments.
[0036]
[0037] In general formula (1), R 1 ~R 5 are each independently a hydrogen atom, an alkoxy group, an alkyl group, a halogen group, a nitro group, a carboxy group, a sulfo group, a phosphate group, a sulfamoyl group, a carbamoyl group, a benzamido group, an alkylsulfamoyl group, an alkylcarbamoyl group, a group represented by the following general formula (101), a group represented by the following general formula (102), or a group represented by the following chemical formula (103), and R 1 ~R 5 cannot all be hydrogen atoms at the same time.
[0038] R 6 ~R 11 are each independently a hydrogen atom, an alkoxy group, an alkyl group, a halogen group, a nitro group, a carboxy group, a sulfo group, a phosphate group, a sulfamoyl group, a carbamoyl group, an alkylsulfamoyl group, an alkylcarbamoyl group, a group represented by the following general formula (104), or a group represented by the following general formula (105), and R 6 ~R 11 cannot all be hydrogen atoms at the same time.
[0039] Here, the "alkoxy group" may have 1 to 8 carbon atoms and may have any of a linear structure, a branched structure, and a cyclic structure. In one embodiment, the alkoxy group preferably has a linear structure. The number of carbon atoms in the alkoxy group is preferably 1 to 4, more preferably 1 or 2, and even more preferably 1.
[0040] The "alkyl group" may have 1 to 18 carbon atoms and may have any of a linear structure, a branched structure, and a cyclic structure. In one embodiment, the alkyl group preferably has a linear structure. The number of carbon atoms in the alkyl group is preferably 1 to 12, more preferably 1 to 8, and even more preferably 1 to 4.
[0041] The "halogen group" may be a fluorine atom, a chlorine atom, or a bromine atom. In one embodiment, a chlorine atom or a fluorine atom is preferred, and a chlorine atom is more preferred.
[0042] The "alkyl" in the "alkylsulfamoyl group" may be the same as the alkyl group described above. The same applies to the "alkyl" in the "alkylcarbamoyl group". Although not particularly limited, in one embodiment, the alkyls in the alkylsulfamoyl group and the alkylcarbamoyl group are each preferably independently an alkyl group having 1 to 4 carbon atoms.
[0043]
[0044] In general formula (101), R 21 ~R 25 are each independently a hydrogen atom, an alkoxy group, an alkyl group, a halogen group, a nitro group, a carboxy group, a sulfo group, a phosphate group, a sulfamoyl group, a carbamoyl group, an alkylsulfamoyl group, an alkylcarbamoyl group, or an aryl group which may have a substituent, or R 21 ~R 25Two adjacent groups among these may combine together to form a saturated or unsaturated alkylene group, or a saturated or unsaturated heteroalkylene group containing one or more heteroatoms selected from the group consisting of oxygen atoms, nitrogen atoms, and sulfur atoms, or form a divalent group having a skeleton composed of a nitrogen atom and a carbonyl group, and the two adjacent groups may combine together with the carbon atoms to which they are bonded to form a ring.
[0045] In the general formula (101), the details of the alkoxy group, the alkyl group, and the halogen group are as described above in the explanation of the general formula (1). The same applies to the alkyl in the alkylsulfamoyl group and the alkylcarbamoyl group.
[0046] In general formula (101), the "aryl group which may have a substituent" refers to an atomic group obtained by removing one hydrogen atom from an aromatic compound. The number of carbon atoms in the aryl group is preferably 6 to 30, more preferably 6 to 18, even more preferably 6 to 12, and particularly preferably 6 to 10. In the aryl group, one or more hydrogen atoms in the aromatic ring may be substituted with a substituent. The substituent may be an alkoxy group, an alkyl group, a halogen group, a nitro group, a carboxy group, a sulfo group, a phosphate group, a sulfamoyl group, a carbamoyl group, an alkylsulfamoyl group, or an alkylcarbamoyl group. Details of these substituents are as described above in the explanation of general formula (1).
[0047] As an embodiment of the structure represented by general formula (101), R 21 ~R 25 Two adjacent groups among R may combine to form a divalent group, and the two adjacent groups may combine to form a ring together with the carbon atoms to which they are bonded. 21 ~R 25 The adjacent two groups are specifically defined as R 21 and R 22 , R 22 and R 23 , R 23 and R 24 , or R24 and R 25 It may be.
[0048] In general formula (101), the carbon atoms to which the two adjacent groups are bonded constitute a benzene ring. Therefore, more specifically, when the two groups are bonded together to form a divalent group, a condensed ring with the benzene ring is formed. Although not particularly limited, the ring formed by the divalent group is preferably a 4-, 5-, or 6-membered ring, more preferably a 5- or 6-membered ring.
[0049] In the embodiment in which a ring is formed as described above, the divalent group formed by two adjacent groups together may be, for example, a saturated or unsaturated alkylene group, a saturated or unsaturated heteroalkylene group, or a saturated or unsaturated group having a skeleton composed of a nitrogen atom and a carbonyl group. When the divalent group is an unsaturated group, it preferably has a conjugated diene structure.
[0050] Examples of the saturated or unsaturated alkylene group include —CH 2 -, -(CH 2 ) 2 -, -CH=CH-CH=CH-, etc. The saturated or unsaturated heteroalkylene group may contain one or more heteroatoms selected from the group consisting of oxygen atoms, nitrogen atoms, and sulfur atoms. The saturated or unsaturated heteroalkylene group may contain 1 to 3 heteroatoms. For example, -O-CH 2 -CH 2 Examples of saturated or unsaturated groups having a skeleton composed of a nitrogen atom and a carbonyl group include a urea bond (-HN-C(=O)-NH-) and an imido bond (-C(=O)-NH-C(=O)-).
[0051] In one embodiment, the divalent group is preferably a group selected from the group consisting of a urea bond (-HN-C(=O)-NH-), an imido bond (-C(=O)-NH-C(=O)-), and a conjugated diene bond (-CH=CH-CH=CH-, -C=N-CH=C-, etc.), with a urea bond being more preferred. When the divalent group is a urea bond, these groups bonded to the carbon atoms constituting the benzene ring together form a benzimidazole ring. Hereinafter, the same specifics apply to cases where substituents bonded to two adjacent carbon atoms constituting a benzene ring together form a divalent group and constitute a ring.
[0052]
[0053] In general formula (102), R 26 ~R 30 are each independently a hydrogen atom, an alkoxy group, an alkyl group, a halogen group, a nitro group, a carboxy group, a sulfo group, a phosphate group, a sulfamoyl group, a carbamoyl group, an alkylsulfamoyl group, an alkylcarbamoyl group, or an aryl group which may have a substituent, or R 26 ~R 30 Two adjacent groups among the above may combine together to form a saturated or unsaturated alkylene group, or a saturated or unsaturated heteroalkylene group containing one or more heteroatoms selected from the group consisting of oxygen atoms, nitrogen atoms, and sulfur atoms, or form a divalent group having a skeleton composed of a nitrogen atom and a carbonyl group, and the two adjacent groups may combine together with the carbon atoms to which they are bonded to form a ring. 26 ~R 30 The details of each group described as are the same as those described above in relation to general formula (101).
[0054]
[0055]
[0056] In general formula (104), R 31 ~R 35are each independently a hydrogen atom, an alkoxy group, an alkyl group, a halogen group, a nitro group, a carboxy group, a sulfo group, a phosphate group, a sulfamoyl group, a carbamoyl group, an alkylsulfamoyl group, an alkylcarbamoyl group, or an aryl group which may have a substituent, or R 31 ~R 35 Two adjacent groups among the above may combine together to form a saturated or unsaturated alkylene group, or a saturated or unsaturated heteroalkylene group containing one or more heteroatoms selected from the group consisting of oxygen atoms, nitrogen atoms, and sulfur atoms, or form a divalent group having a skeleton composed of a nitrogen atom and a carbonyl group, and the two adjacent groups may combine together with the carbon atoms to which they are bonded to form a ring. 31 ~R 35 The details of each group described as are the same as those described above in relation to general formula (101).
[0057]
[0058] In general formula (105), R 36 ~R 40 are each independently a hydrogen atom, an alkoxy group, an alkyl group, a halogen group, a nitro group, a carboxy group, a sulfo group, a phosphate group, a sulfamoyl group, a carbamoyl group, an alkylsulfamoyl group, an alkylcarbamoyl group, or an aryl group which may have a substituent, or R 36 ~R 40 Two adjacent groups among the above may combine together to form a saturated or unsaturated alkylene group, or a saturated or unsaturated heteroalkylene group containing one or more heteroatoms selected from the group consisting of oxygen atoms, nitrogen atoms, and sulfur atoms, or form a divalent group having a skeleton composed of a nitrogen atom and a carbonyl group, and the two adjacent groups may combine together with the carbon atoms to which they are bonded to form a ring. 36 ~R 40 The details of each group described as are the same as those described above in relation to general formula (101).
[0059] In one embodiment, the average primary particle diameter of compound (A) is preferably 1,000 nm or less, more preferably 350 nm or less, and even more preferably 200 nm or less. Furthermore, the average primary particle diameter of compound (A) is preferably 10 nm or more, more preferably 30 nm or more, and even more preferably 50 nm or more. The average primary particle diameter can be determined by calculating the average of the longer diameters of 50 primary pigment particles extracted from multiple photographs taken with a transmission electron microscope at a magnification of 10,000 times. When the average primary particle diameter of compound (A) is within the optimal range, it becomes easy to achieve both coloring power and dispersibility.
[0060] In one embodiment, compound (A) may be a compound known as a naphthol-based azo pigment and may be commercially available. Examples of commercially available compounds (A) include C.I. Pigment Red 5, 8, 10, 17, 22, 23, 31, 32, 114, 146, 147, 150, 170, 176, 185, 208, 245, 258, 268, and 269, and C.I. Pigment Violet 32 and 50. One or a combination of two or more of these compounds may be used as compound (A). In one embodiment, compound (A) is preferably a monoazo pigment containing one azo bond in the molecule.
[0061] In one embodiment, the compound (A) preferably contains at least one selected from the group consisting of C.I. Pigment Red 17, 22, 23, 31, 32, 114, 146, 147, 150, 176, 185, 245, 258, and 269. In one embodiment, the compound (A) more preferably contains at least one selected from the group consisting of C.I. Pigment Red 31, 32, 146, 147, 150, 176, and 269. In one embodiment, the compound (A) preferably contains two or more of the above C.I. Pigment Red pigments. Specific examples of combinations of two pigments include C.I. Pigment Red 269 / Red 150, Red 150 / Red 31, and Red 146 / Red 147. Here, the term "C.I." stands for Color Index number.
[0062] In one embodiment, the compound (A) preferably has the following structure: In general formula (1), R 1 ~R 5 are each independently a group selected from the group consisting of a hydrogen atom, an alkyl group, a carboxy group, and a carbamoyl group, and contain at least one carboxy group or one carbamoyl group. 6 ~R 11 is a group represented by general formula (104), and R in general formula (104) 31 ~R 35 are each independently a group selected from the group consisting of a hydrogen atom, an alkoxy group, and a halogen group, and contain at least one alkoxy group or one halogen group.
[0063] <Compound (B)> In the colorant of the above embodiment, the compound (B) is a compound having a structure represented by the following general formula (2).
[0064] In general formula (2), R 1 '~R 5 ' are each independently a hydrogen atom, an alkoxy group, an alkyl group, a halogen group, a nitro group, a carboxy group, a sulfo group, a phosphate group, a sulfamoyl group, a carbamoyl group, a benzamido group, an alkylsulfamoyl group, an alkylcarbamoyl group, a group represented by the general formula (101), a group represented by the general formula (102), or a group represented by the chemical formula (103), and R 1 '~R 5 In one embodiment, R 1 '~R 5 ' represents R at the corresponding position in compound (A). 1 ~R 5 and preferably match each other. That is, for example, R 1 and R 1 ', R 2 and R 2 In such a relationship, R 1 ~R 5 and the corresponding R 1 '~R 5X' are preferably the same group as each other. X is a hydrogen atom, a hydroxyl group, or a chlorine atom. In one embodiment, X is preferably a hydrogen atom.
[0065] In one embodiment, the compound (A) and the compound (B) in the colorant are preferably compounds defined as follows in the above general formula (1) and the above general formula (2): 1 ~R 5 and R 1 '~R 5 Each of R ′ independently represents a hydrogen atom, an alkoxy group, an alkyl group, a nitro group, a carboxy group, a carbamoyl group, a benzamido group, an alkylsulfamoyl group, a group represented by the general formula (101) above, or a group represented by the chemical formula (103) above. 6 ~R 11 are each independently a hydrogen atom, a carbamoyl group, or a group represented by the above general formula (104).
[0066] In one embodiment, the compound (A) and the compound (B) are preferably compounds defined as follows in the general formula (1) and the general formula (2): 1 ~R 5 At least two of R are a combination of two different groups selected from the group consisting of an alkoxy group, an alkyl group, a nitro group, a carbamoyl group, a benzamido group or an alkylsulfamoyl group, a group represented by the general formula (101) above, and a group represented by the chemical formula (103) above. 1 '~R 5 At least two of R' are a combination of two different groups selected from the group consisting of an alkoxy group, an alkyl group, a nitro group, a carbamoyl group, a benzamido group or an alkylsulfamoyl group, a group represented by the general formula (101) above, and a group represented by the chemical formula (103) above. 1 '~R 5 ' are R at the corresponding positions 1 ~R 5 and R are preferably the same groups. 6 ~R 11 At least one of the groups is a carbamoyl group or a group represented by the above general formula (104).
[0067] In the above embodiment, in the above general formula (101), R 21 ~R 25 are each preferably a hydrogen atom. 31 ~R 35 are each independently a hydrogen atom, an alkoxy group, an alkyl group, a halogen group, or a nitro group, or R 31 ~R 35 It is preferred that two adjacent groups in the above formula (I) combine to form a urea bond.
[0068] In one embodiment, R in the general formula (1) 1 ~R 5 In the formula (101), the combinations of two different groups are preferably each independently an alkyl group / nitro group, an alkoxy group / nitro group, an alkoxy group / group represented by the above general formula (101), an alkoxy group / alkylsulfamoyl group, an alkoxy group / carbamoyl group, or an alkoxy group / alkylsulfamoyl group.
[0069] The R in the general formula (2) 1 '~R 5 In R′, the combination of two different groups is preferably an alkyl group / nitro group, an alkoxy group / nitro group, an alkoxy group / group represented by the above general formula (101), an alkoxy group / alkylsulfamoyl group, an alkoxy group / carbamoyl group, or an alkoxy group / alkylsulfamoyl group. 1 '~R 5 ' are R at the corresponding positions 1 ~R 5 and are preferably the same groups.
[0070] In the colorant of the above embodiment, compound (A) preferably includes a compound represented by the following general formula (3). Also, compound (B) preferably includes a compound represented by the following general formula (4). From this perspective, it is more preferable that the colorant includes a compound represented by the following general formula (3) and a compound represented by the following general formula (4).
[0071]
[0072] In general formula (3), R 6 ~R 11 are each independently a hydrogen atom, an alkoxy group, an alkyl group, a halogen group, a nitro group, a carboxy group, a sulfo group, a phosphate group, a sulfamoyl group, a carbamoyl group, an alkylsulfamoyl group, an alkylcarbamoyl group, a group represented by general formula (104), or a group represented by general formula (105), and R 6 ~R 11 cannot all be hydrogen atoms at the same time. 6 ~R 11 The details of each group described as are the same as those described above in the explanation of general formula (1).
[0073]
[0074] In the general formula (4), X is a hydrogen atom, a hydroxyl group, or a chlorine atom. In one embodiment, X is preferably a hydrogen atom.
[0075] In one embodiment, the compound (A) and the compound (B) in the colorant are preferably compounds defined as follows in the above general formula (1) and the above general formula (2): 1 ~R 5 and R 1 '~R 5 Each of R ′ independently represents a hydrogen atom, an alkyl group, a carboxy group, or a carbamoyl group, and contains at least one carboxy group or one carbamoyl group. 1 '~R 5 ' are R at the corresponding positions 1 ~R 5 and R are preferably the same groups. 6 is a group represented by the above general formula (104), and R 7 ~R 11 is a hydrogen atom. In the above general formula (104), R 31 ~R 35 are each independently a hydrogen atom, an alkoxy group, or a halogen group, and R 31 ~R 35 cannot all be hydrogen atoms at the same time.
[0076] The main component of the colorant of the above embodiment is compound (A), which is known as a naphthol-based azo pigment, and the colorant further contains compound (B). The content of compound (A) in the colorant may be 50% by mass or more, based on the total mass of the colorant. From the viewpoint of easily obtaining the coloring strength of compound (A), the content may be preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more. On the other hand, the content may be 99.99% by mass or less. From the viewpoint of easily improving dispersibility and optical properties, the content may be preferably 99.9% by mass or less, more preferably 99.7% by mass or less, and even more preferably 99.5% by mass or less.
[0077] In one embodiment, from the viewpoint of facilitating improvements in the coloring power and optical properties of the colorant, the content of the compound (A) based on the total mass of the colorant may be preferably 80 to 99.9 mass%, more preferably 90 to 99.7 mass%, and even more preferably 95 to 99.5 mass%. Here, the content of the compound (A) in the colorant can be calculated, for example, by absorptiometry, as described in the Examples below.
[0078] The colorant of the above embodiment further contains the compound (B) in addition to the compound (A) as the main component, thereby improving dispersibility, clarity, and transparency. The inventors speculate that the presence of compound (B) in the colorant causes the aromatic ring portion of compound (B) to adsorb to the surface of compound (A), making the surface of compound (A) (pigment) hydrophobic. As a result, the dispersion stability of the pigment in the dispersion can be easily improved. Therefore, for example, when an aqueous dispersion is prepared using the colorant, good dispersion stability and viscosity stability can be easily obtained. The reason for this is speculated to be that the presence of compound (B) in the colorant or on the surface of compound (A) suppresses the growth of pigment crystal particles.
[0079] In the colorant, the content of compound (B) relative to the total mass of compound (A) may be 0.001% by mass or more. In one embodiment, from the viewpoint of facilitating improvement of optical properties, the content may preferably be 0.01% by mass or more. The content may be, for example, 0.02% by mass, 0.03% by mass, 0.04% by mass, 0.05% by mass, or 0.06% by mass. In one embodiment, the content may more preferably be 0.1% by mass or more. The content may be, for example, 0.15% by mass, 0.2% by mass, 0.25% by mass, 0.3% by mass, 0.35% by mass, 0.36% by mass, 0.4% by mass, or 0.45% by mass. The content may further preferably be 0.5% by mass or more, and particularly preferably 0.52% by mass or more.
[0080] On the other hand, from the viewpoint of coloring power, the content may preferably be 10.0% by mass or less. The content may be 5.4% by mass or less, 5.3% by mass or less, or 5.22% by mass or less. In one embodiment, the content may more preferably be 1.6% by mass or less. The content may be, for example, 1.5% by mass or less, 1.4% by mass or less, 1.3% by mass or less, 1.2% by mass or less, or 1.1% by mass or less. In one embodiment, the content may further preferably be 1.0% by mass or less, even more preferably 0.9% by mass or less, particularly preferably 0.65% by mass or less, and particularly preferably 0.64% by mass or less.
[0081] When the content of compound (B) relative to the total mass of compound (A) is adjusted to fall within the above range, the optical properties of the coating film, such as clarity, gloss, and transparency, can be easily improved. Furthermore, the color stability of the colorant against alkali can be easily maintained. Furthermore, the color stability of dispersions such as various printing inks using the colorant and the viscosity stability of the dispersions during storage at varying temperatures can be easily maintained.
[0082] In one embodiment, the colorant may further contain other components in addition to the compound (A) and the compound (B), to the extent that desired properties can be maintained. For example, the colorant may further contain components derived from raw materials used in the production of the colorant in addition to the compound (A) and the compound (B).
[0083] In one embodiment, the colorant may further contain a compound (C) represented by the following general formula (5).
[0084] In general formula (5), R 1 ~R 5 are each independently a hydrogen atom, an alkoxy group, an alkyl group, a halogen group, a nitro group, a carboxy group, a sulfo group, a phosphate group, a sulfamoyl group, a carbamoyl group, an alkylsulfamoyl group, an alkylcarbamoyl group, a group represented by the general formula (101) above, a group represented by the general formula (102) above, or a group represented by the chemical formula (103) above, and R 1 ~R 5 cannot all be hydrogen atoms at the same time. 1 ~R 5 The details of each group described as are the same as those described above in the explanation of general formula (101).
[0085] In the colorant, the content of compound (C) relative to the total mass of compound (A) may preferably be 0.001% by mass or more. In one embodiment, the content may be 0.005% by mass or more, or 0.007% by mass or more. The content may more preferably be 0.01% by mass or more. In one embodiment, the content may be 0.02% by mass. The content may further preferably be 0.03% by mass or more.
[0086] On the other hand, the content may be preferably 0.5% by mass or less, more preferably 0.46% by mass or less, and even more preferably 0.15% by mass or less. The content may be, for example, 0.14% by mass, 0.13% by mass, or 0.12% by mass. In one embodiment, the content of compound (C) may be 0% by mass.
[0087] When the colorant contains compound (C) in the above range, the coloring power and transparency tend to be more easily improved. Furthermore, the dispersion stability in a solvent-based dispersion tends to be further improved. Therefore, in one embodiment, the colorant contains compound (A), compound (B), and compound (C), and the content of compound (C) is preferably 0.001 to 0.5% by mass relative to the total mass of compound (A). The content may be more preferably 0.01 to 0.46% by mass, and even more preferably 0.03 to 0.12% by mass.
[0088] In one embodiment, the colorant may further contain a compound (D) represented by the following general formula (6):
[0089] In general formula (6), R 1 ~R 5 are each independently a hydrogen atom, an alkoxy group, an alkyl group, a halogen group, a nitro group, a carboxy group, a sulfo group, a phosphate group, a sulfamoyl group, a carbamoyl group, an alkylsulfamoyl group, an alkylcarbamoyl group, a group represented by the general formula (101) above, a group represented by the general formula (102) above, or a group represented by the chemical formula (103) above, and R 1 ~R 5 cannot all be hydrogen atoms at the same time. 1 ~R 5 The details of each group described as are the same as those described above in the explanation of general formula (101).
[0090] The content of compound (D) relative to the total mass of compound (A) may be 0.001% by mass or more. When the colorant contains compound (D), transparency and coloring power tend to be more easily improved. On the other hand, the content of compound (D) in the colorant is preferably 0.12% by mass or less. By adjusting the content of compound (D) to 0.12% by mass or less, thickening due to excessive particle size reduction can be easily suppressed. Therefore, the content of compound (D) relative to the total mass of compound (A) is preferably in the range of 0.001% by mass to 0.12% by mass.
[0091] In one embodiment, particularly when the colorant is used for coloring or printing for textile and food packaging applications, a low content of compound (D) is preferred. In consideration of use in the above applications, the content of compound (D) in the colorant may preferably be 0.12% by mass or less. The content may more preferably be 0.005% by mass or less.
[0092] In one embodiment, the colorant may further contain a compound (E) represented by the following general formula (7):
[0093] In general formula (7), R 6 ~R 11 are each independently a hydrogen atom, an alkoxy group, an alkyl group, a halogen group, a nitro group, a carboxy group, a sulfo group, a phosphate group, a sulfamoyl group, a carbamoyl group, an alkylsulfamoyl group, an alkylcarbamoyl group, a group represented by the general formula (104), or a group represented by the general formula (105), and R 6 ~R 11 cannot all be hydrogen atoms at the same time. 6 ~R 11 The details of each group described as are the same as those described above in the explanation of general formula (101).
[0094] The content of compound (E) relative to the total mass of compound (A) may be 0.001% by mass or more. When the colorant contains compound (E), aggregation of primary particles tends to be suppressed, making it easier to improve dispersibility. On the other hand, the content of compound (E) in the colorant is preferably 6% by mass or less. By adjusting the content of compound (E) in the colorant to 6% by mass or less, it is possible to easily suppress a decrease in coloring power, printability, and coating film properties in various ink applications. For example, in inkjet ink applications, it is possible to easily suppress a decrease in discharge performance due to precipitation of compound (E). Furthermore, in gravure ink applications, it is possible to easily suppress a decrease in lamination strength. Furthermore, in active energy ray-curable ink applications, it is possible to easily avoid problems such as inhibition of curability and a decrease in storage stability.
[0095] Therefore, in one embodiment, when the colorant is used for ink or ink applications, it is preferable that the content of compound (E) in the colorant is low. When considering use in the above applications, the content of compound (E) in the colorant may preferably be 5.9% by mass or less. The content may more preferably be 1.3% by mass or less, and even more preferably be 1.1% by mass or less. The content may be, for example, 1.0% by mass, 0.9% by mass, 0.8% by mass, 0.7% by mass, 0.6% by mass, 0.5% by mass, 0.4% by mass, 0.3% by mass, or 0.1% by mass. In one embodiment, the content may be 0% by mass.
[0096] In one embodiment, the content of the compound (E) in the colorant may be 0.01% by mass to 5.88% by mass, more preferably 0.01% by mass to 1.26% by mass, and even more preferably 0.01% by mass to 0.88% by mass.
[0097] As described above, in one embodiment, the colorant contains the compound (A) and the compound (B), and may further contain one or more compounds selected from the group consisting of the compound (C), the compound (D), and the compound (E). Here, the colorant of the above embodiment preferably satisfies one or more of the following requirements (i) to (iii): (i) the content of the compound (C) relative to the total mass of the compound (A) is 0.001% by mass or more and 0.5% by mass or less; (ii) the content of the compound (D) relative to the total mass of the compound (A) is 0.12% by mass or less; and (iii) the content of the compound (E) relative to the total mass of the compound (A) is 6% by mass or less.
[0098] In yet another embodiment, the colorant may further contain other components in addition to compound (A) and compound (B), and optionally at least one selected from the group consisting of compounds (C), (D), and (E), as long as the desired properties can be maintained. For example, during the production of an insoluble azo pigment, components such as a resin and / or a surfactant may be used for the purpose of surface modification of the pigment. The colorant of the above embodiment does not require surface modification because it has excellent dispersibility due to the presence of compound (B). However, as described below, components such as a resin or a surfactant may also be used as needed during the production of the colorant. In this case, the colorant may further contain the resin or surfactant used as needed.
[0099] In one embodiment, when a resin is used in the production of a colorant, the content of the resin may preferably be 0.1 to 10% by mass relative to the total mass of the colorant (colorant being 100% by mass). The content of the resin may more preferably be 0.5 to 5% by mass, and even more preferably be 1 to 3% by mass. Furthermore, when a surfactant is used in the production of a colorant, the content of the surfactant may preferably be 0.1 to 10% by mass relative to the total mass of the colorant (colorant being 100% by mass). The content of the surfactant may more preferably be 0.5 to 5% by mass, and even more preferably be 1 to 3% by mass.
[0100] When the colorant of the above embodiment further contains a component other than the compound (A) and the compound (B), the content thereof may be preferably 20% by mass or less, more preferably 10% by mass or less, and even more preferably 5% by mass or less, based on the total mass of the colorant. When the content is adjusted to the above range, the good properties achieved by the interaction between the compound (A) and the compound (B) can be easily maintained.
[0101] <2> Manufacturing Method of Colorant The manufacturing method of the colorant of the above embodiment is not particularly limited. For example, a colorant can be manufactured by adding compound (B) to compound (A) and mixing them. Examples of methods for adding compound (B) include a method of manufacturing compound (B) in the presence of compound (A), a method of separately manufacturing compound (A) and compound (B) and mixing them, and a method of manufacturing compound (A) in the presence of compound (B), and any of these methods can be selected. The method of manufacturing compound (A) in the presence of compound (B) is preferred because it allows a colorant with high transparency to be easily obtained. The method of manufacturing compound (B) in the presence of compound (A) is also preferred because it allows a colorant with high dispersion stability to be easily obtained.
[0102] In producing the colorant, compound (A) can be produced by applying a known synthesis method for insoluble azo pigments. For example, a coupling reaction between a base component and a coupler component can be applied. More specifically, an aromatic amine represented by the following general formula (6) is diazotized as the base component to prepare a solution (1) containing a diazonium salt represented by the following general formula (6A). Furthermore, a solution (2) containing a coupler component represented by the following general formula (7) is prepared. These solutions (1) and (2) are then mixed to carry out a coupling reaction between the base component and the diazonium salt. Compound (A) can be produced by carrying out such a coupling reaction.
[0103]
[0104] R in the above general formulas (6) and (6A) 1 ~R 5 is as explained above.
[0105]
[0106] R in the above general formula (7) 6 ~R 11 is as explained above.
[0107] In the colorant of the above embodiment, when compound (A) contains two or more compounds, for example, a solution containing two or more coupler components is prepared, and a coupling reaction between this solution and a solution containing a diazonium salt is carried out to obtain the desired two or more compounds. In another embodiment, a first solution containing only the first coupler component and a second solution containing only the second coupler component may be prepared, and the coupling reaction may be carried out stepwise. Similarly, a solution containing a diazonium salt using two or more base components is prepared, and a coupling reaction between this solution and a solution containing a coupler component is carried out to obtain the desired two or more compounds.
[0108] Both the solution containing the diazonium salt and the solution containing the coupler component contain at least water. The solution may be in the form of a transparent aqueous solution or a suspension, but is preferably in the form of an aqueous solution. In one embodiment, the coupling reaction is preferably carried out in the presence of a water-soluble organic solvent. From this perspective, the solution containing the diazonium salt and / or the solution containing the coupler component preferably further contains a water-soluble organic solvent in addition to water. In one embodiment, the solution containing at least the coupler component preferably contains water and a water-soluble organic solvent. When a water-soluble organic solvent is used, the solubility of the coupler component is improved, which tends to increase the reactivity and yield.
[0109] The solution containing the coupler component contains the coupler component, a base, and water, and may further contain a water-soluble organic solvent as needed. The solution containing the coupler component can be prepared, for example, by dissolving the coupler component in a heated basic aqueous solution. As another example, the solution may be prepared by mixing water, a water-soluble organic solvent, the coupler component, and a base at room temperature (approximately 10°C to 30°C) and dissolving the coupler component and the base. The dissolution temperature can be adjusted depending on the type and amount of water-soluble organic solvent, the amount of water, and the type and amount of base to be added. For example, when the solution contains a water-soluble organic solvent, mixing is preferably carried out at approximately 15 to 50°C. When the solution does not contain a water-soluble organic solvent, mixing is preferably carried out at 50 to 95°C.
[0110] The base may be, for example, soluble in water and capable of dissolving the coupler component. Furthermore, a base that does not form an insoluble salt when neutralized with an acid in an aqueous acid solution or a solution containing a diazonium salt, as described below, is preferred. Such a base is advantageous in terms of cost, dissolving power of the coupler component, waste liquid treatment, etc. Examples of preferred bases include sodium hydroxide and potassium hydroxide.
[0111] The solution containing the diazonium salt contains the diazonium salt and water. The solution containing the diazonium salt may contain a reaction mixture of the base component used in preparing the diazonium salt, an acid component, and aqueous sodium nitrite. The diazonium salt can be obtained by diazotizing the base component of the general formula (6) above. Known methods can be used for diazotization. For example, diazotization can be carried out by adding hydrochloric acid or sulfuric acid to a solution obtained by slurrying the base component with ice water, dissolving the solution, and then adding sodium nitrite. Sulfamic acid may be added to eliminate excess sodium nitrite used for diazotization. A water-soluble organic solvent can be added to the solution containing the diazonium salt.
[0112] The water-soluble organic solvent that can be used during the coupling reaction is not particularly limited. Any organic solvent that can be arbitrarily mixed with water may be used. A water-soluble organic solvent can be used to obtain a solution containing a coupler component and / or a solution containing a diazonium salt. Examples of water-soluble organic solvents include aprotic polar solvents such as acetonitrile, dimethyl sulfoxide, N,N-dimethylformamide, and N-methyl-2-pyrrolidone; ketones such as acetone and methyl ethyl ketone; cyclic ethers such as tetrahydrofuran and 1,4-dioxane; dihydric alcohols such as ethylene glycol, diethylene glycol, and polyethylene glycol; and monohydric alcohols such as methanol, ethanol, and isopropanol.
[0113] The water-soluble organic solvent may be one of the above solvents used alone or a combination of two or more of them. Although not particularly limited, the water-soluble organic solvent preferably includes at least one selected from the group consisting of aprotic polar solvents, ketones, monohydric alcohols, and cyclic ethers. Furthermore, the boiling point of the water-soluble organic solvent is preferably 100°C or lower. Such water-soluble organic solvents with a boiling point of 100°C or lower are advantageous in terms of solvent recovery from waste liquid. For example, at least one selected from the group consisting of acetonitrile, acetone, methanol, and tetrahydrofuran can be suitably used.
[0114] The amount of the water-soluble organic solvent added can be adjusted depending on the type of water-soluble organic solvent. In one embodiment, whether the water-soluble organic solvent is added to the solution containing the coupler component or the solution containing the diazonium salt, the amount added is preferably 1 to 50 mass% relative to the total mass of the slurry after coupling (out of 100 mass%). The amount of the water-soluble organic solvent added is more preferably 7 to 30 mass%, and even more preferably 12 to 21 mass%.
[0115] Examples of the coupling method include reverse coupling, forward coupling, acid precipitation forward coupling, etc. Among these, reverse coupling, which will be described later, is preferred from the viewpoints of particle size control and reaction yield.
[0116] A known method can be used for the reverse coupling. For example, a method of adding a solution containing a coupler component to a solution containing a diazonium salt can be used. The temperature during coupling is preferably 0 to 50°C. From the viewpoints of suppressing alteration and decomposition of the diazonium salt and of reaction rate, a temperature of 10 to 30°C is particularly preferred.
[0117] A buffer solution may be added in advance to the solution containing the diazonium salt. The type of buffer solution is not particularly limited, and any solution having buffering ability may be used. For example, it is preferable to use an aqueous solution of acetic acid and sodium acetate. When a buffer solution is added, it is preferable to adjust the pH of the solution containing the diazonium salt to a range of 3.0 to 6.5. From the viewpoint of improving the reaction rate and dispersibility, it is preferable to heat the slurry after coupling as necessary.
[0118] The compound (B) in the colorant can be produced by a known method. For example, the compound (B) can be derived from the raw material used to produce the compound (A). In this case, R 1 '~R 5 ' are R in the general formula (1) at the corresponding positions, respectively. 1 ~R 5 and have the same base.
[0119] In view of the above, in one embodiment, a method for producing a colorant includes carrying out a coupling reaction between a solution containing a coupler component represented by general formula (7) and a solution containing a diazonium salt represented by general formula (6A) obtained by diazotizing an aromatic amine, using a diazonium salt in a molar ratio that is in excess of the coupler component. As described above, when an excess amount of diazonium salt is used in the coupling reaction, compound (B) can be produced by thermal decomposition of a portion of the diazonium salt. Therefore, according to the production method of the above embodiment, compound (B) can be produced together with compound (A).
[0120] Here, an excessive amount of diazonium salt means that the ratio of the molar amount (y) of the diazonium salt to the molar amount (x) of the coupler component (i.e., the molar ratio (y) / (x)) is greater than 1. For example, in a mixed solution of a solution containing a coupler component and a solution containing a diazonium salt, the molar ratio (y) / (x), calculated as "the molar amount (y) of the diazonium salt in the solution / the molar amount (x) of the coupler component in the solution," is preferably adjusted to be 1.01 or more and 1.1 or less. In one embodiment, the molar ratio (y) / (x) is more preferably 1.015 or more and 1.06 or less. When the molar ratio (y) / (x) is adjusted to be within the above range, it becomes easy to adjust the content of compound (B) in the colorant to be within a preferred range.
[0121] In the production method of the above embodiment, the coupling reaction is preferably carried out in the presence of a water-soluble organic solvent. Therefore, the solution containing the coupler component and the solution containing the diazonium salt each contain at least water and may further contain a water-soluble organic solvent as necessary. In the production method of the above embodiment, it is particularly preferable that the solution containing at least the coupler component contains a water-soluble organic solvent.
[0122] In the production method of the above embodiment, if the molar amount of the diazonium salt is excessive relative to the molar amount of the coupler component, the solubility of the coupler component tends to decrease when the solutions are mixed for the coupling reaction. However, by using a water-soluble organic solvent, the coupler component can be easily dissolved, which tends to facilitate the production of a colorant with a high yield. Furthermore, although the reason is unclear, when the thermal decomposition of an excess amount of diazonium salt is carried out in the presence of a water-soluble organic solvent, compound (B) tends to be efficiently produced.
[0123] The decomposition of the excess diazonium salt can be carried out by heating the solution after the coupling reaction or by irradiating it with light. Either method may be used, but the method of heating the solution after the coupling reaction is preferred. As long as the diazonium salt can be decomposed, the heating temperature and heating time are not limited and can be adjusted appropriately. In one embodiment, from the viewpoint of the time required for treatment, the heating temperature is preferably 45°C or higher, more preferably 55°C or higher, and even more preferably 65°C or higher. On the other hand, from the viewpoint of energy cost, the heating temperature is preferably 95°C or lower, more preferably 85°C or lower, and even more preferably 75°C or lower. In one embodiment, the heating time is preferably about 30 minutes to 4 hours, more preferably 30 minutes to 2 hours, and even more preferably 30 minutes to 1 hour.
[0124] The pH of the mixed solution when heated is not particularly limited as long as it can decompose the diazonium salt. In one embodiment, the pH of the mixed solution is preferably 2 or higher, more preferably 3 or higher, and even more preferably 4 or higher. The pH of the mixed solution is preferably 7 or lower, more preferably 6 or lower, and even more preferably 5 or lower. Here, the mixed solution refers to a solution obtained by mixing a solution containing a coupling component and a solution containing a diazonium salt, and is also referred to as a reaction solution.
[0125] When the mixed solution is adjusted to the pH range and heated, the unreacted coupler component and the diazonium salt first react to produce compound (A), and then the excess diazonium salt (remaining in the reaction mixture) decomposes to produce compound (B). Thus, when the coupling reaction is carried out under the above conditions, compound (B) adsorbs to the surface of compound (A), thereby suppressing crystal growth of pigment particles during subsequent heating, stirring, and drying, and thus easily producing a pigment with high transparency and excellent dispersion stability. Furthermore, after heating under the above heating conditions, the pH may be adjusted before filtration in order to improve purification efficiency. The acids and bases used to adjust the pH may be the same as those used in preparing the solution containing the coupler component, the solution containing the diazonium salt, and the buffer solution described above, and these can be used preferably.
[0126] In another embodiment, a method for producing a colorant may be employed in which compound (A) is produced in the presence of compound (B). In this case, compound (B) is preferably added to a solution containing a coupler component. When a colorant is produced by such a method, a colorant with high transparency can be easily obtained even with a small amount of compound (B).
[0127] The colorant slurry obtained by the coupling reaction is preferably subjected to removal of water, solvent, water-soluble salts, etc. using a known suction filter, filter press, ultrafilter, etc. In this manner, a colorant press cake can be easily obtained. The colorant press cake may be washed with water, an organic solvent, or other solvent, as needed. The colorant press cake can be used as is to produce a coloring composition. A powder coloring composition can be produced and used by drying and pulverizing the colorant press cake according to a known method.
[0128] In one embodiment, a well-known technique for producing a naphthol azo pigment can be applied to produce the colorant. For example, when producing the colorant, components known to those skilled in the art can be used in addition to the pigment raw materials, as needed. For example, well-known components such as a resin and / or a surfactant can be used to be present in the colorant.
[0129] In one embodiment, the well-known components may be added to a solution containing a coupler component, a solution containing a diazonium salt, or an acid solution for acid precipitation. When the well-known components are added to a solution containing a coupler component, they may be added before or after dissolving the coupler component. In another embodiment, the well-known components may be added to a slurry obtained after the coupling reaction. Alternatively, the well-known components may be added to a pigment press cake obtained by filtering and washing the pigment after the coupling reaction, and then reslurried.
[0130] If components such as a resin and / or a surfactant are used during the production of a colorant, these remain on the surface of the colorant even after production. Therefore, it is preferable that the resin and / or surfactant be hydrophilic or have the property of dissolving in a basic solution. The use of such a resin and / or surfactant tends to improve dispersibility by alleviating aggregation of the colorant and to facilitate imparting affinity of the colorant to the dispersing resin and solvent selected depending on the application. The colorant of the above embodiment does not necessarily require the above component because the presence of compound (B) provides excellent dispersibility. However, the use of the above component can also provide manufacturing benefits such as improved reactivity due to the promotion of dissolution of the coupler component and suppression of crystal growth of the pigment in the colorant.
[0131] Resins that can be used for the above purposes include, for example, styrene-(meth)acrylic acid copolymers, (meth)acrylic acid-(meth)acrylic acid alkyl ester copolymers, styrene-(meth)acrylic acid-(meth)acrylic acid alkyl ester copolymers, styrene-α-methylstyrene-(meth)acrylic acid copolymers, styrene-α-methylstyrene-(meth)acrylic acid-(meth)acrylic acid alkyl ester copolymers, polyacrylic acid, polymethacrylic acid, vinylnaphthalene-(meth)acrylic acid copolymers, styrene-maleic acid (anhydride) copolymers, maleic acid-maleic anhydride copolymers, vinylnaphthalene-maleic acid (anhydride) copolymers, α-olefin-maleic acid (anhydride) copolymers, α-olefin-maleic acid alkyl ester copolymers, resins having acid groups such as polyester-modified acrylic acid polymers, acrylic copolymers, and salts thereof. The above resins may be used alone or in combination of two or more.
[0132] When the above-mentioned resin is used in the production of a colorant, a compound capable of forming a salt with the above-mentioned resin can be further used. For example, a basic compound such as an inorganic base or an organic base can be used. Examples of inorganic bases include alkali metal hydroxides such as lithium hydroxide, sodium hydroxide, and potassium hydroxide; alkali metal silicic acid salts such as sodium orthosilicate, sodium metasilicate, and sodium sesquisilicate; alkali metal phosphates such as trisodium phosphate; alkali metal carbonates such as disodium carbonate, sodium bicarbonate, and dipotassium carbonate; alkali metal boric acid salts such as sodium borate; and ammonia.
[0133] Examples of organic bases include alkylamines such as methylamine, dimethylamine, trimethylamine, ethylamine, diethylamine, and triethylamine, alkanolamines such as aminoethanol, methylaminoethanol, dimethylaminoethanol, ethylaminoethanol, butylaminoethanol, diethylaminoethanol, dibutylaminoethanol, diethanolamine, and triethanolamine, and amines having a nonionic group such as methoxypoly(oxyethylene / oxypropylene)-2-propylamine. The basic compounds may be used alone or in combination of two or more.
[0134] In yet another embodiment, a surfactant can be used in the preparation of the colorant. The surfactant can be, for example, an anionic, nonionic, or amphoteric surfactant.
[0135] Examples of anionic surfactants include fatty acid salts, alkyl sulfate ester salts, alkylaryl sulfonates, alkylnaphthalenesulfonates, alkyl sulfates, dialkyl sulfonates, dialkyl sulfosuccinates, alkyl diaryl ether disulfonates, alkyl phosphates, polyoxyethylene alkyl ether sulfates, polyoxyethylene alkylaryl ether sulfates, naphthalenesulfonate-formalin condensates, polyoxyethylene alkyl ether phosphates, polyoxyethylene alkyl phosphate ester salts, glycerol borate fatty acid esters, and polyoxyethylene glycerol fatty acid esters.
[0136] Examples of amphoteric surfactants include betaine, sulfobetaine, alkylbetaine, and alkylamine oxide.
[0137] Examples of nonionic surfactants include polyoxyethylene alkyl ethers, polyoxyethylene alkylaryl ethers, polyoxyethylene oxypropylene block copolymers, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, polyoxyethylene sorbitol fatty acid esters, glycerin fatty acid esters, polyoxyethylene fatty acid esters, and polyoxyethylene alkylamines.
[0138] In one embodiment, among the above surfactants, a combination of an amphoteric surfactant and an anionic surfactant is preferred. Although not particularly limited, when a surfactant is added to a solution containing a coupler component, an anionic or amphoteric surfactant is preferred. When a surfactant is added to a slurry obtained after the coupling reaction, a nonionic surfactant may be used. The surfactants may be used alone or in combination of two or more.
[0139] <3> Coloring Composition One embodiment of the present invention relates to a coloring composition containing the colorant of the above embodiment. In the coloring composition, components other than the colorant can be selected appropriately depending on the application. In one embodiment, the coloring composition for use in forming a coating film may contain a dispersion medium in addition to the colorant, and the dispersion medium may contain at least one or more compounds selected from the group consisting of a resin and a polymerizable compound. The dispersion medium may further contain a solvent.
[0140] In the coloring composition, the dispersion medium is selected depending on the application of the coloring composition. In one embodiment, the coloring composition contains a colorant and a resin, and may further contain a solvent as needed. In another embodiment, the coloring composition contains a colorant and a polymerizable compound, and may further contain at least one of a resin and a solvent as needed. Each of the coloring compositions of the above embodiments may further contain various additives as needed. Examples of coloring compositions include pigment dispersions, toners, paints, and printing inks. Hereinafter, the coloring composition will be described in more specific embodiments.
[0141] <Pigment Dispersion> In one embodiment, the coloring composition may be in the form of a colorant dispersion (hereinafter referred to as "pigment dispersion") containing the colorant of the above embodiment as a main component and further containing a dispersion medium for dispersing the colorant. The dispersion medium contains at least a resin and may further contain a solvent depending on the application. The pigment dispersion can be suitably used, for example, as a masterbatch for coloring plastics. The masterbatch contains at least a colorant and a resin and is suitable for coloring plastic molded bodies. The pigment dispersion can also be suitably used, for example, as an intermediate for paints, printing inks, and the like. The pigment dispersion used as the intermediate may contain a colorant, a resin, and a solvent. The resin contained in the pigment dispersion may contain a resin-type pigment dispersant.
[0142]
[0033] When the pigment dispersion is used for various applications, it is preferable that the viscosity is not likely to increase and that the pigment dispersion has excellent dispersion stability. The pigment dispersion of this embodiment is superior to conventional pigment dispersions containing naphthol-based azo pigments in that it has excellent dispersibility and a low initial viscosity. Furthermore, the pigment dispersion of this embodiment is also superior in terms of hue stability against alkalis and viscosity stability during storage at varying temperatures.
[0143] When the pigment dispersion contains a solvent, the solvent may be water, a water-soluble solvent, or a water-insoluble solvent. When the solvent contains at least water, an aqueous pigment dispersion can be formed. The water-soluble solvent and the water-insoluble solvent are not particularly limited. For example, they may be the same as the water-soluble solvent and the water-insoluble solvent that constitute the paint described below.
[0144] The disperser used to prepare the aqueous pigment dispersion is not particularly limited. Examples of dispersers include horizontal sand mills, vertical sand mills, annular bead mills, attritors, microfluidizers, high-speed mixers, homomixers, homogenizers, high-pressure homogenizers, ball mills, paint shakers, roll mills, stone mills, ultrasonic dispersers, high-pressure dispersers, opposed collision dispersers, and oblique collision dispersers. In addition, dispersers and mixers that are commonly used in the art to prepare various dispersions can be appropriately selected and used.
[0145] Furthermore, prior to dispersion, treatments such as pre-dispersion using a milling mixer such as a kneader or a three-roll mill, or solid dispersion using a two-roll mill, etc. may be carried out. Furthermore, after dispersion using various dispersers, post-treatments such as storage in a heated state at 30 to 80°C for several hours to about one week, or post-treatments using an ultrasonic disperser or a collision-type beadless disperser may be carried out, and these processes are effective in imparting dispersion stability to the pigment dispersion.
[0146] <Toner> In one embodiment, the coloring composition can be suitably used in toner applications. The toner coloring composition contains the colorant of the above embodiment and a dispersion medium (resin). The toner coloring composition may further contain components well known to those skilled in the art as toner components, such as a charge control agent.
[0147] The toner may be either a dry toner or a liquid toner. The toner coloring composition may also be used to prepare toner according to other methods known in the art.
[0148] The resin constituting the toner coloring composition is not particularly limited. Examples include styrene-acrylic acid ester copolymers, styrene-based copolymers, polyester resins, etc. These resins are also called binder resins.
[0149] In one embodiment, the binder resin for the toner is preferably a polyester resin or a styrene copolymer, and more preferably a polyester resin. The colorant of this embodiment is particularly suitable for polyester resins among the above binder resins. Therefore, in one embodiment, the toner coloring composition preferably contains a colorant and a binder resin containing a polyester resin. In such a toner coloring composition, the colorant of the above embodiment is uniformly and finely dispersed in the binder resin containing a polyester resin. Therefore, the coloring composition of the above embodiment can provide a high-quality toner.
[0150] <Paint> In one embodiment, the coloring composition can be suitably used in paint applications. The coloring composition for paint contains the colorant, resin, and solvent of the above embodiment. The coloring composition for paint is preferably prepared using a pigment dispersion containing a colorant, resin, and solvent. For example, the coloring composition for paint can be prepared by mixing the pigment dispersion, a resin for paint, and a solvent. Here, the resin in the pigment dispersion and the resin used to prepare the paint may be the same or different.
[0151] Thermosetting resins and / or thermoplastic resins can be used as resins for coating materials. The thermosetting resin is preferably a resin with a glass transition temperature of 10°C or higher. Examples of thermosetting resins include acrylic resins, polyester resins, polyurethane resins, and melamine resins. Furthermore, the thermosetting resin preferably has a functional group that can react with a curing agent. Examples of the functional group include a carboxyl group and a hydroxyl group. Examples of curing agents include an isocyanate curing agent, an epoxy curing agent, an aziridine curing agent, and an amine curing agent. The thermoplastic resin is preferably a resin with a glass transition temperature of 30°C or higher. Examples of thermoplastic resins include nitrocellulose resins, acrylic resins, and polyester resins. A thermosetting resin and a thermoplastic resin may be used in combination.
[0152] The solvent may be water, a water-insoluble solvent, or a water-soluble solvent. When the solvent contains at least water, it can constitute an aqueous paint. Specific examples of water-insoluble solvents include toluene, xylene, butyl acetate, methyl acetate, methyl isobutyl ketone, and aliphatic hydrocarbons. The water-soluble solvent may be, for example, a monohydric alcohol or a dihydric alcohol. Examples of water-soluble solvents include monohydric alcohols such as ethanol, n-propanol, isopropanol, and isobutanol; dihydric alcohols such as ethylene glycol, diethylene glycol, triethylene glycol, and propylene glycol; and trihydric or higher polyhydric alcohols such as glycerin. The water-soluble solvent may be a water-dilutable monoether derived from a polyhydric alcohol, such as methoxypropanol or methoxybutanol. Other examples include water-dilutable glycol ethers such as butyl glycol and butyl diglycol. In one embodiment, from the perspective of constituting an aqueous paint, the solvent preferably contains both water and a water-soluble solvent.
[0153] In one embodiment, the paint may further contain a luster material. The luster material may be particles having an average thickness of 0.5 to 10 μm and an average particle size of 5 to 50 μm. Examples of luster materials include metal flakes, mica, and coated glass flakes. Examples of metal flakes include aluminum flakes and gold powder. Examples of mica include regular mica and coated mica. Examples of coated glass flakes include glass flakes coated with a metal oxide such as titanium oxide. The content of the luster material is preferably 0.1 to 10% by mass relative to the total mass of the paint (out of 100% by mass).
[0154] The paint may further contain other components. For example, color pigments and various additives commonly used in the art may be blended as necessary. The method for producing the paint and the methods for applying and drying the paint are not particularly limited, and methods well known in the art can be applied. Examples of uses of the paint include paint for metals and paint for plastics.
[0155] <Printing Ink> In one embodiment, the coloring composition can be suitably used in printing ink applications. The coloring composition for printing ink contains the colorant of the above embodiment and a dispersion medium, and the dispersion medium is appropriately selected depending on the type of printing ink. Printing inks can be broadly classified into solvent-based printing inks, water-based printing inks, and actinic energy ray-curable printing inks depending on the presence or absence of a solvent and the type of dispersion medium. Printing inks can also be further subdivided depending on the printing format, for example, into offset printing inks, flexographic printing inks, gravure printing inks, color filter inks, inkjet printing inks, etc. The colorant of this embodiment has excellent dispersibility, coloring power, clarity, and transparency, and can therefore be suitably used in various printing ink applications. Representative printing inks will be exemplified below.
[0156] In one embodiment, the printing ink contains the colorant, resin, and solvent of the above embodiment. These printing inks are distinguished from the actinic radiation-curable printing inks described below. Examples of such printing inks include offset printing inks, flexographic printing inks, gravure printing inks, and color filter inks. Hereinafter, these various printing inks will be abbreviated as flexographic inks, gravure inks, color filter inks, and inkjet inks. Note that when the solvent constituting the printing ink contains at least water, it is referred to as an aqueous printing ink.
[0157] The printing ink coloring composition is preferably prepared using a pigment dispersion containing a colorant, a resin, and a solvent. For example, the printing ink coloring composition can be prepared by mixing the pigment dispersion, a printing ink resin, and a solvent. Here, the resin in the pigment dispersion and the resin used to prepare the printing ink may be the same or different.
[0158] In the printing ink of the above embodiment, the resin may be, for example, a rosin resin, a rosin-modified phenolic resin, polyurethane, nitrocellulose, an acrylic resin, a styrene-acrylic resin, or a petroleum resin.
[0159] In the printing ink of the above embodiment, the solvent may be water, a water-insoluble solvent, or a water-soluble solvent, such as toluene, xylene, butyl acetate, methyl acetate, methyl ethyl ketone, methyl isobutyl ketone, butyl alcohol, or an aliphatic hydrocarbon.
[0160] Examples of water-soluble solvents include ethanol, n-propanol, isopropanol, isobutanol, ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, and glycerin. Also included are water-dilutable monoethers derived from polyhydric alcohols. Examples include methoxypropanol and methoxybutanol. Also included are water-dilutable glycol ethers such as butyl glycol and butyl diglycol. In one embodiment, from the viewpoint of forming an aqueous printing ink, the solvent contains at least water. The solvent may further contain either a water-insoluble solvent or a water-soluble solvent. In one embodiment, the solvent preferably contains water and a water-soluble solvent.
[0161] The printing ink may further contain a luster material. The type and amount of the luster material may be as exemplified above in the description of the paint.
[0162] The printing ink may contain other components. For example, color pigments and various additives commonly used in the art may be blended as necessary. The method for producing the printing ink and the methods for applying and drying it are not particularly limited, and methods well known in the art can be used.
[0163] Inkjet Ink In one embodiment, the coloring composition can be suitably used as an ink for inkjet (IJ) printing. Hereinafter, inkjet (IJ) printing ink will be abbreviated as IJ ink. In one embodiment, the coloring composition for IJ ink contains a colorant and a resin. In another embodiment, the coloring composition for IJ ink preferably contains a colorant and a resin, and further contains a solvent. The coloring composition for IJ ink is preferably prepared using a pigment dispersion containing a colorant, a resin, and, if necessary, a solvent. In another embodiment, the coloring composition for IJ ink may be a composition in which the resin in the coloring composition for IJ ink of the previously described embodiment is changed to a polymerizable compound, or a composition in which a resin and a polymerizable compound are used in combination. For example, the coloring composition for IJ ink can be prepared by mixing the pigment dispersion with a resin for IJ ink. Here, the resin in the pigment dispersion and the resin used to prepare the IJ ink may be the same or different.
[0164] Inkjet inks can be broadly classified into (solvent-based) inkjet inks, aqueous inkjet inks, and actinic radiation-curable inkjet inks depending on the presence or absence of a solvent and the type of solvent, and the type of resin or polymerizable compound used as the dispersion medium. Actinic radiation-curable inkjet inks can be further classified into photocurable inkjet inks and electron beam-curable inkjet inks depending on the curing method used to cure the polymerizable compound. Although not particularly limited, the coloring composition of the above embodiment can be suitably used as an aqueous inkjet ink. Below, an aqueous inkjet ink will be described as an example of an inkjet ink.
[0165] The content of the colorant is preferably 0.5 to 30% by mass, and more preferably 1 to 15% by mass, with the total mass of the water-based inkjet ink being 100% by mass.
[0166] The resin used in aqueous inkjet inks is important for achieving ink fixation to the printed material (substrate). Examples of resins include acrylic resins, olefin-maleic acid resins, styrene-acrylic resins, polyester resins, polyamide resins, and polyurethane resins. The resin may be in the form of, for example, a water-soluble resin or emulsion particles. Of these, emulsion particles are preferred. The emulsion particles may be, for example, particles of a single composition or core-shell particles, and can be selected as desired. The use of emulsion particles makes it easy to reduce the viscosity of aqueous inkjet inks, making it easy to obtain printed materials with excellent water resistance.
[0167] The resin content in the aqueous inkjet ink is preferably 2 to 30% by mass, and more preferably 3 to 20% by mass, based on 100% by mass of the nonvolatile content. When the inkjet ink contains a resin within the above range, the ejection stability and fixability tend to be improved.
[0168] From the viewpoint of forming an aqueous inkjet ink, the solvent contains at least water. The solvent may further contain either a water-insoluble solvent or a water-soluble solvent. In one embodiment, the solvent preferably contains water and a water-soluble solvent. Examples of water-soluble solvents include glycol ethers and diols. These solvents penetrate into substrates very quickly, even into substrates with low or no liquid absorption.
[0169] Examples of low-absorbency or non-absorbency substrates include coated paper, art paper, vinyl chloride sheets, films, and fabrics. When a solvent with excellent permeability to the substrate is used as described above, drying during printing is fast, and accurate printing can be easily achieved. Furthermore, when a water-soluble solvent with a high boiling point is used, the solvent also acts as a wetting agent.
[0170] The water-soluble solvent is important for preventing the aqueous inkjet ink from drying and solidifying in the nozzle portion of the printer head and for achieving ink ejection stability. From this perspective, examples of water-soluble solvents that can be suitably used include ethylene glycol, diethylene glycol, propylene glycol, triethylene glycol, polyethylene glycol, glycerin, tetraethylene glycol, dipropylene glycol, ketone alcohol, diethylene glycol monobutyl ether, ethylene glycol monobutyl ether, ethylene glycol monoethyl ether, 1,2-hexanediol, N-methyl-2-pyrrolidone, substituted pyrrolidone, 2,4,6-hexanetriol, tetrafurfuryl alcohol, and 4-methoxy-4-methylpentanone.
[0171] In one embodiment, the total content of water and the water-soluble solvent is preferably 15 to 50% by mass relative to 100% by mass of the inkjet ink. Here, the content of the water-soluble solvent may be preferably 10 to 90% by mass, more preferably 20 to 80% by mass, and even more preferably 30 to 70% by mass, relative to the total mass of water and the water-soluble solvent.
[0172] The inkjet ink may further contain additives such as drying accelerators, penetrants, preservatives, chelating agents, pH adjusters, antifoaming agents, wetting agents, and surfactants.
[0173] In one embodiment, the inkjet ink is particularly suitable for use as a magenta ink. The inkjet ink may be combined with inks of colors other than magenta to form an ink set. Examples of colors that can be combined with the inkjet ink include cyan, yellow, black, white, red, green, blue, orange, pink, gold, silver, and bronze.
[0174] The ink set may be, for example, a four-color ink set that adds cyan, yellow, and black to the magenta inkjet ink used in the above embodiment. In other embodiments, it may be suitably used as an ink set of five or more colors by adding special colors such as orange, red, and green. The pigment concentration, viscosity, dynamic viscoelasticity, surface tension, coating order, evaporation rate of volatile components, etc. of each ink are design factors and can be adjusted appropriately depending on the desired characteristics.
[0175] The inkjet ink of the above embodiment can be applied to a variety of conventionally known substrates, including highly water-absorbent substrates such as plain paper, fabric, and knitted fabric, low-absorbent substrates such as art paper, coated paper, vinyl chloride, wood, concrete, polyethylene film, polypropylene film, polyethylene terephthalate film, natural leather, and artificial leather, and non-water-absorbent substrates such as metals (aluminum, stainless steel, etc.).
[0176] <Actinic Energy Ray-Curable Flexographic Ink> In one embodiment, the coloring composition can be configured as an active energy ray-curable flexographic printing ink. Hereinafter, an active energy ray-curable flexographic printing ink will be abbreviated as active energy ray-curable flexographic ink. Aimed at such printing ink applications, the coloring composition for active energy ray-curable flexographic ink contains the colorant of the above embodiment and a polymerizable compound as a dispersion medium. It may also contain a photopolymerization initiator. The content of the colorant in the active energy ray-curable flexographic ink is not particularly limited. In one embodiment, the content of the colorant is preferably 5 to 30 mass %, more preferably 10 to 25 mass %, relative to the total mass of the ink.
[0177] In the ink of the above embodiment, the polymerizable compound is preferably a compound having one or more ethylenically unsaturated bonds in the molecule, and the polymerizable compound contains a monomer and / or an oligomer (hereinafter, "monomer and / or oligomer" will be abbreviated simply as "monomer").
[0178] The monomer preferably has a polymerizable group such as a (meth)acryloyl group, an allyl group, a vinyl group, a vinyl ether group, etc. In terms of curability, the monomer preferably contains a monomer having either a (meth)acryloyl group or a vinyl group, more preferably contains a monomer having 3 to 6 (meth)acryloyl groups in the molecule, and even more preferably contains a monomer having 6 (meth)acryloyl groups in the molecule.
[0179] The monomer having a (meth)acryloyl group is not particularly limited, but examples thereof include the following: Trifunctional (meth)acrylate monomers having three (meth)acryloyl groups in the molecule: trimethylolpropane tri(meth)acrylate, EO-modified (3) trimethylolpropane tri(meth)acrylate, EO-modified (6) trimethylolpropane tri(meth)acrylate, PO-modified (3) trimethylolpropane tri(meth)acrylate, ε-caprolactone-modified tris-(2-acryloxyethyl)isocyanurate, ethoxylated isocyanuric acid tri(meth)acrylate, tris(2-hydroxyethyl)isocyanurate tri(meth)acrylate, pentaerythritol tri(meth)acrylate, etc. Tetrafunctional (meth)acrylate monomers having four acryloyl groups in the molecule: pentaerythritol tetra(meth)acrylate, EO-modified (4) pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, etc. Pentafunctional (meth)acrylate monomers having five (meth)acryloyl groups in the molecule: dipentaerythritol penta(meth)acrylate, etc. Hexafunctional (meth)acrylate monomers having six (meth)acryloyl groups in the molecule: dipentaerythritol hexa(meth)acrylate, etc.
[0180] Examples of the monomer having a vinyl group include N-vinyl-2-pyrrolidone and N-vinylcaprolactam.
[0181] Examples of the oligomer include urethane (meth)acrylate oligomers such as aliphatic urethane (meth)acrylate oligomers and aromatic urethane (meth)acrylate oligomers, (meth)acrylic ester oligomers, polyester (meth)acrylate oligomers, and epoxy (meth)acrylate oligomers. The oligomer preferably contains about 2 to 16 ethylenically unsaturated bonds. Among these, urethane (meth)acrylate oligomers are preferred, and urethane (meth)acrylate oligomers having 6 to 12 (meth)acryloyl groups are more preferred. The hexa- to 12-functional urethane (meth)acrylate oligomers are also commercially available.
[0182] The weight-average molecular weight (Mw) of the oligomer is preferably 400 to 10,000, more preferably 500 to 5,000, more preferably 800 to 4,000, and even more preferably 1,000 to 2,000. Here, the "weight-average molecular weight (Mw)" can be determined as a polystyrene-equivalent molecular weight by standard gel permeation chromatography (hereinafter, GPC). In the ink of the above embodiment, one polymerizable compound may be used alone, or two or more polymerizable compounds may be used in combination. The content of the polymerizable compound is preferably 25 to 90% by mass, more preferably 35 to 80% by mass, based on the total mass of the active energy ray-curable flexographic ink.
[0183] In one embodiment, the actinic ray-curable flexographic ink contains a compound having one or more ethylenically unsaturated bonds in the molecule as a polymerizable compound, and when light is used as the actinic ray, it preferably contains a photopolymerization initiator. The photopolymerization initiator preferably contains a radically polymerizable photopolymerization initiator. The photopolymerization initiator undergoes a chemical change to generate radicals by the action of light, or, when a sensitizing dye is used in combination, by photoelectron transfer or energy transfer with the sensitizing dye.
[0184] The photoradical polymerization initiator is not particularly limited, and known ones can be used, such as benzophenone-based compounds, dialkoxyacetophenone-based compounds, α-hydroxyalkylphenone-based compounds, α-aminoalkylphenone-based compounds, acylphosphine oxide-based compounds, and thioxanthone-based compounds.
[0185] The polymerization initiators may be used alone or in combination of two or more. The content of the polymerization initiator is preferably 0.5 to 20% by mass, more preferably 5 to 15% by mass, based on the total mass of the active energy ray-curable flexographic ink.
[0186] In one embodiment, the active energy ray-curable flexographic ink may also contain a polymerization initiator aid. By containing a polymerization initiator aid, curability can be further improved. Examples of the polymerization initiator aid include triethanolamine, methyldiethanolamine, triisopropanolamine, aliphatic amines, ethyl 2-dimethylaminobenzoate, ethyl 4-dimethylaminobenzoate, isoamyl 4-dimethylaminobenzoate, and dibutylethanolamine.
[0187] The content of the polymerization initiator aid is preferably 0.1 to 5% by mass, more preferably 0.5 to 3% by mass, based on the total mass of the active energy ray-curable flexographic ink.
[0188] In one embodiment, the active energy ray-curable flexographic ink preferably contains a wax to further improve abrasion resistance, anti-blocking properties, smoothness, and scratch resistance. The wax is not particularly limited, and known waxes can be used. Examples include natural waxes and synthetic waxes. Examples of natural waxes include carnauba wax, Japan wax, lanolin, montan wax, paraffin wax, and microcrystalline wax. Examples of synthetic waxes include Fischer-Tropsch wax, polyethylene wax, polypropylene wax, polytetrafluoroethylene wax, polyamide wax, and silicone compounds.
[0189] From the viewpoint of the balance between abrasion resistance, gloss, and piling, the content of the wax is preferably 0.1 to 5 mass %, more preferably 0.5 to 4 mass %, based on the total mass of the active energy ray-curable flexographic ink.
[0190] In one embodiment, the active energy ray-curable flexographic ink may further contain a resin as a dispersion medium in addition to the polymerizable compound. The inclusion of a resin mitigates cure shrinkage of the coating film that occurs during curing, suppresses curling of the substrate, and further facilitates improving adhesion to the substrate.
[0191] Examples of resins include polyvinyl chloride, poly(meth)acrylic acid ester, epoxy resin, polyester resin, polyurethane resin, cellulose derivatives (e.g., ethyl cellulose, cellulose acetate, nitrocellulose), vinyl chloride-vinyl acetate copolymer, polyamide resin, polyvinyl acetal resin, diallyl phthalate resin, alkyd resin, rosin-modified alkyd resin, rosin-modified alkyd resin, petroleum resin, urea resin, and synthetic rubber such as butadiene-acrylonitrile copolymer. Of these, diallyl phthalate resin and polyester resin are preferred. Diallyl phthalate resin is more preferred.
[0192] The weight average molecular weight of the resin is preferably 1,000 to 100,000, and more preferably 2,000 to 70,000.
[0193] The above resins may be used alone or in combination of two or more. From the viewpoint of curability, the content of the resin is preferably 1 to 15% by mass, more preferably 1 to 5% by mass, based on the total mass of the active energy ray-curable flexographic ink.
[0194] In one embodiment, the active energy ray-curable flexographic ink may contain a polymerization inhibitor, such as 4-methoxyphenol, hydroquinone, methylhydroquinone, t-butylhydroquinone, 2,6-di-t-butyl-4-methylphenol, phenothiazine, and aluminum salt of N-nitrosophenylhydroxylamine.
[0195] The content of the polymerization inhibitor is preferably 0.01 to 2% by mass relative to the total mass of the active energy ray-curable flexographic ink, from the viewpoint of maintaining the curability while improving the storage stability of the active energy ray-curable flexographic ink.
[0196] The active energy ray-curable flexographic ink may contain other components such as various additives in addition to the above components, as needed, to the extent that the effects of the present invention are not impaired. Various additives, such as extender pigments, leveling agents, surfactants, antifoaming agents, UV absorbers, antistatic agents, and antioxidants, can be added to the ink as needed. Furthermore, the colorant of the above embodiment does not necessarily require a dispersant because it has excellent dispersibility due to the presence of compound (B) in addition to compound (A). However, from the perspective of further improving dispersibility, the active energy ray-curable flexographic ink may contain a well-known dispersant as needed.
[0197] It is preferable that the active energy ray-curable flexographic ink contains substantially no water, where "substantially no water" means that the content of water in the ink composition is 1% by mass or less.
[0198] One embodiment of the present invention relates to an article such as a printed matter having a coating film composed of the paint or printing ink of the above embodiment. The printed matter can be formed according to a method well known in the art. For example, in the case of an actinic energy ray-curable flexographic ink, the ink can be printed on a recording medium by flexographic printing, and then the ink can be cured by irradiating it with actinic energy rays to form the printed matter.
[0199] The recording medium is not particularly limited, and known recording media can be used, including coated paper such as art paper, coated paper, and cast paper, uncoated paper such as fine paper, medium-quality paper, and newsprint, synthetic paper such as Yupo paper, and plastic films such as PET (polyethylene terephthalate), PP (polypropylene), and OPP (biaxially oriented polypropylene).
[0200] The method for curing the active energy ray-curable flexographic ink is not particularly limited, and known methods can be used. For example, the ink can be cured by irradiating it with α-rays, γ-rays, electron beams, X-rays, ultraviolet light, visible light, infrared light, or the like. Of these, ultraviolet light and electron beams are preferred, and ultraviolet light is more preferred. The peak wavelength of the active energy ray is preferably 200 to 600 nm, and more preferably 350 to 420 nm.
[0201] The active energy ray source is not particularly limited, and known sources can be used. Specific examples include mercury lamps, xenon lamps, metal hydride lamps, LEDs (light-emitting diodes) such as ultraviolet light-emitting diodes (UV-LEDs) and ultraviolet laser diodes (UV-LDs), and gas / solid-state lasers. Among these, ultraviolet light-emitting diodes (UV-LEDs) are preferred because of their small size, long life, high efficiency, and low cost.
[0202] Although the embodiments of the present invention have been described above, the present invention is not limited to the above-described embodiments and includes various other embodiments.
[0203] The present invention will be described in more detail below with reference to examples. The present invention is not limited to the following examples. Unless otherwise specified, "parts" means "parts by mass" and "%" means "% by mass".
[0204] The abbreviations and product names used in the following examples have the following meanings. <Couplers> Naphthol AS: 3-hydroxy-2-naphthanilide Naphthol AS-BI: 5-(3-hydroxy-2-naphthoylamino)benzimidazolone Naphthol AS-BS: 3-hydroxy-3'-nitro-2-naphthanilide Naphthol AS-CA: N-(5-chloro-2-methoxyphenyl)-3-hydroxy-2-naphthamide Naphthol AS-D: 3-hydroxy-2'-methyl-2-naphthanilide Naphthol AS-KB: 5'-chloro-3-hydroxy-2'-methyl-2-naphthanilide Naphthol AS-LC: 4'-chloro-3-hydroxy-2',5'-dimethoxy-2-naphthanilide BON amide: 3-hydroxy-2-naphthamide BON acid: 3-hydroxy-2-naphthoic acid Naphthol AS-RL: 3-hydroxy-4'-methoxy-2-naphthanilide Naphthol AS-OL: 3-hydroxy-2'-methoxy-2-naphthanilide Naphthol AS-E: 4'-chloro-3-hydroxy-2-naphthanilide
[0205] <Base> M-20: 3-amino-4-methoxybenzamide M-40: 3-amino-4-methoxybenzanilide M-60: 3-amino-4-methylbenzamide R185 Base: 4-amino-5-methoxy-N,2-dimethylbenzenesulfonamide V32 Base: 4-amino-2,5-dimethoxy-N-methylbenzenesulfonamide Azoic DC31: 4-benzylsulfonyl-2-aminomethoxybenzene First Scarlet G: 2-methyl-5-nitroaniline First Scarlet RC: 2-methoxy-5-nitroaniline First Violet B: 4-benzoylamino-2-methoxy-5-methylaniline M-70: 4-aminobenzamide
[0206] <Compound (A)> C.I. Pigment Red 269: N-(5-chloro-2-methoxyphenyl)-3-hydroxy-4-[2-methoxy-5-(phenylcarbamoyl)phenylazo]-2-naphthamide C.I. Pigment Red 150: 3-hydroxy-4-((2-methoxy-5-((phenylamino)carbonyl)phenyl)azo)-2-naphthalenecarboxamide C.I. Pigment Red 31: 4-((5-(anilino)carbonyl-2-methoxyphenyl)azo)-3-hydroxy-N-(3-nitrophenyl)naphthalene-2-carboxamide C.I. Pigment Red 17: 3-hydroxy-4-((2-methyl-5-nitrophenyl)azo)-N-(2-methylphenyl)-2-naphthalenecarboxamide C.I. Pigment Red 22: 3-hydroxy-4-((2-methyl-5-nitrophenyl)azo)-N-phenyl-2-naphthalenecarboxamide C.I. Pigment Red 23: 1-(2-methoxy-5-nitrophenylazo)-2-hydroxy-3-(3-nitrophenylcarbamoyl)naphthalene C.I. Pigment Red 32: 4-((5-(anilino)carbonyl-2-methoxyphenyl)azo)-3-hydroxy-N-phenylnaphthalene-2-carboxamide C.I. Pigment Red 266: 4-((4-(aminocarbonyl)phenyl)azo)-3-hydroxy-N-(2-methoxyphenyl)naphthalene-2-carboxamide Compound (A)-1: 4-((5-carbamoyl-2-methylphenyl)azo)-3-hydroxy-N-(4-methoxyphenyl)naphthalene-2-carboxamide Compound (A)-2: 4-((4-(aminocarbonyl)phenyl)azo)-3-hydroxy-N-(4-methoxyphenyl)naphthalene-2-carboxamide Compound (A)-3: 4-((4-carboxyphenyl)azo)-3-hydroxy-N-(4-methoxyphenyl)naphthalene-2-carboxamide Compound (A)-4: 4-((5-carbamoyl-2-methylphenyl)azo)-3-hydroxy-N-(2-methoxyphenyl)naphthalene-2-carboxamideCompound (A)-5: 4-((4-carboxyphenyl)azo)-3-hydroxy-N-(2-methoxyphenyl)naphthalene-2-carboxamide Compound (A)-6: 4-((4-carboxyphenyl)azo)-3-hydroxy-N-(4-chlorophenyl)naphthalene-2-carboxamide
[0207] C.I. Pigment Red 114: 1-(2-methyl-5-nitrophenylazo)-2-hydroxy-3-(3-nitrophenylcarbamoyl)naphthalene C.I. Pigment Red 146: N-(4-chloro-2,5-dimethoxyphenyl)-3-hydroxy-4-((2-methoxy-5-((phenylamino)carbonyl)phenyl)azo)naphthalene-2-carboxamide C.I. Pigment Red 147: 3-hydroxy-4-((2-methoxy-5-((phenylamino)carbonyl)phenyl)azo)-N-(5-chloro-2-methylphenyl)-2-naphthalenecarboxamide C.I. Pigment Red 176: N-(2,3-dihydro-2-oxo-1H-benzimidazol-5-yl)-3-hydroxy-4-((2-methoxy-5-((phenylamino)carbonyl)phenyl)azo)naphthalene-2-carboxamide C.I. Pigment Red 185: N-(2,3-dihydro-2-oxo-1H-benzimidazol-5-yl)-2-hydroxy-4-((2-methoxy-5-methyl-4-((methylamino)sulfonyl)phenyl)azo)naphthalene-2-carboxamide C.I. Pigment Red 245: 4-((5-carbamoyl-2-methoxyphenyl)azo)-3-hydroxy-N-phenylnaphthalene-2-carboxamide C.I. Pigment Red 258: 4-((5-benzylsulfonyl-2-methoxyphenyl)azo)-3-hydroxy-N-phenylnaphthalene-2-carboxamide C.I. Pigment Red 268: 4-((5-carbamoyl-2-methylphenyl)azo)-3-hydroxy-N-phenylnaphthalene-2-carboxamide C.I. Pigment Violet 32: N-(2,3-dihydro-2-oxo-1H-benzimidazol-5-yl)-2-hydroxy-4-((2,5-dimethoxy-4-((methylamino)sulfonyl)phenyl)azo)naphthalene-2-carboxamide C.I. Pigment Violet 50: 4-((4-(anilino)carbonyl-2-methoxyphenyl-3-methyl)azo)-3-hydroxy-N-phenylnaphthalene-2-carboxamide
[0208] <Compound (B)> 4MPB: 4-methoxy-N-phenylbenzamide (manufactured by Wako Pure Chemical Industries, Ltd.) 4MB: 4-methylbenzamide (manufactured by Wako Pure Chemical Industries, Ltd.) 4MBA: 4-methoxybenzamide (manufactured by Wako Pure Chemical Industries, Ltd.) p-nitrotoluene (manufactured by Wako Pure Chemical Industries, Ltd.) 4-nitroanisole (manufactured by TCI) DA-FVB: N-(5-methoxy-2-methylphenyl)benzamide DA-DC31: 1-(benzylsulfonyl)-4-methoxybenzene DA-R185: 5-methoxy-N,2-dimethylbenzenesulfonamide DA-V32: 2,5-dimethoxy-N-methylbenzenesulfonamide benzamide (manufactured by Tokyo Chemical Industry Co., Ltd.) Benzoic acid (manufactured by Tokyo Chemical Industry Co., Ltd.)
[0209] <1> Preparation of Colorants (Example 1) Preparation of Colorant 1 237.4 parts of 3-amino-4-methoxybenzanilide as a base component was added to 3,518 parts of water and stirred to prepare a suspension, to which 1,465 parts of ice was added to adjust the temperature to 5°C or below. 389.0 parts of 35% hydrochloric acid was added and stirred for 30 minutes. Subsequently, an aqueous solution prepared by adding 69.9 parts of sodium nitrite to 104.8 parts of water was added, and the mixture was stirred for 1 hour to carry out diazotization. Sulfamic acid was added to the reaction mixture obtained by the above diazotization, and excess nitrous acid was removed. Sulfamic acid was added until no free nitrous acid was detected using potassium iodide paper. 203.0 parts of sodium acetate and 22.4 parts of 80% acetic acid were added to the suspension to prepare a solution containing a diazonium salt.
[0210] Separately, a mixture of 1639 parts of methanol, 199.0 parts of a 40% aqueous sodium hydroxide solution, and 62.0 parts of water was adjusted to 15 to 25°C. 327.8 parts of naphthol AS-CA was added and dissolved therein as a coupler component. 0.9 parts of 4-methoxy-N-phenylbenzamide (manufactured by Wako Pure Chemical Industries, Ltd.) was then added as compound (B) to form a coupler solution. This solution was added over 20 minutes to a solution containing a diazonium salt adjusted to 25°C, and a coupling reaction was carried out.
[0211] The slurry obtained by the coupling reaction was stirred for 1 hour, then heated to 70°C and stirred at 68 to 72°C for an additional 1 hour. The pH at this time was 4.5. A 40% aqueous solution of sodium hydroxide was added to adjust the pH to 10.5 to 11.5, and the mixture was stirred for an additional 15 minutes. The slurry was cooled to 50°C or below, filtered, and washed with water to obtain a press cake of the colorant. The press cake was dried at 80°C for 18 hours and then pulverized to obtain 561.2 parts of Colorant 1.
[0212] Examples 2 to 17 Production of Colorants 2 to 17 Colorants 2 to 17 were obtained in the same manner as in Example 1, except that 237.4 parts of 3-amino-4-methoxybenzanilide as the base component was changed to the corresponding base type and base parts by mass in Table 1, 327.8 parts by mass of naphthol AS-CA as the coupler component was changed to the corresponding first coupler type and first coupler parts by mass in Table 1, and 0.9 parts by mass of compound (B) was changed to the corresponding part by mass in Table 1.
[0213] Example 18: Preparation of Colorant 18 245.9 parts of 3-amino-4-methoxybenzanilide as a base component was added to 3,643 parts of water and stirred to prepare a suspension. 1,517 parts of ice was then added and the temperature was adjusted to 5°C or below. 402.9 parts of 35% hydrochloric acid was added thereto and stirred for 30 minutes. Subsequently, an aqueous solution prepared by adding 72.3 parts of sodium nitrite to 108.5 parts of water was added and stirred for 1 hour to carry out diazotization. Sulfamic acid was added to the reaction mixture to remove excess nitrous acid. Sulfamic acid was added until no free nitrous acid was detected using potassium iodide paper. 210.2 parts of sodium acetate and 23.2 parts of 80% acetic acid were added to the mixture to prepare a solution containing a diazonium salt.
[0214] Separately, a mixture of 1639 parts of methanol, 199.0 parts of a 40% aqueous sodium hydroxide solution, and 62.0 parts of water was adjusted to 15 to 25°C. 327.8 parts of naphthol AS-CA was added and dissolved therein as a coupler component to prepare a coupler solution. This solution was added over 20 minutes to a solution containing a diazonium salt that had been adjusted to 25°C, to carry out a coupling reaction.
[0215] The slurry obtained by the coupling reaction was stirred for 1 hour, then heated to 70°C and stirred at 68-72°C for an additional 1 hour. At this time, the pH was 4.5. A 40% aqueous solution of sodium hydroxide was added to adjust the pH to 10.5-11.5, and the mixture was stirred for an additional 15 minutes. The slurry was cooled to below 50°C, filtered, and washed with water to obtain a press cake of colorant. The press cake was dried at 80°C for 18 hours and then pulverized to obtain 573.2 parts of Colorant 18.
[0216] Examples 19 to 34 Production of Colorants 19 to 34 Colorants 19 to 34 were obtained in the same manner as in Example 18, except that 245.9 parts of 3-amino-4-methoxybenzanilide as the base component was changed to the corresponding base type and base parts by mass in Table 1, and 327.8 parts by mass of naphthol AS-CA as the coupler component was changed to the corresponding first coupler type and first coupler parts by mass in Table 1.
[0217] Example 35: Preparation of Colorant 35 A solution containing a diazonium salt was prepared in the same manner as in Example 18. Separately, a mixture of 1,475 parts of methanol, 179.1 parts of a 40% aqueous sodium hydroxide solution, and 55.8 parts of water was adjusted to 15 to 25°C. 295.0 parts of naphthol AS-CA was added and dissolved therein as a first coupler component to prepare a first coupler solution. Furthermore, a mixture of 164 parts of methanol, 19.9 parts of a 40% aqueous sodium hydroxide solution, and 6.2 parts of water was adjusted to 15 to 25°C. 18.7 parts of BONamide was added and dissolved therein as a second coupler component to prepare a second coupler solution. The first coupler solution was added to the diazonium salt solution adjusted to 25°C over 18 minutes, and then the second coupler solution was added over 2 minutes to carry out a coupling reaction.
[0218] The slurry obtained by the coupling reaction was stirred for 1 hour, then heated to 70°C and stirred at 68-72°C for an additional 1 hour. The pH was 4.5 at this time. A 40% aqueous solution of sodium hydroxide was added to adjust the pH to 10.5-11.5, and the mixture was stirred for an additional 15 minutes. The slurry was cooled to below 50°C, filtered, and washed with water to obtain a press cake of colorant. The press cake was dried at 80°C for 18 hours and then pulverized to obtain 559.2 parts of Colorant 35.
[0219] (Examples 36 to 39) Production of Colorants 36 to 39 Colorants 36 to 39 were obtained in the same manner as in Example 35, except that naphthol AS-CA was used as the first coupler component, with the first coupler type and first coupler parts by mass shown in the table, and BON amide was used as the second coupler component, with the second coupler type and second coupler parts by mass shown in the table. The solution used to dissolve the coupler, the amount of base, and the time required for coupling were changed appropriately depending on the amounts of the first coupler and second coupler.
[0220] Example 40: Production of Colorant 40 As the coupler component, 327.8 parts of Naphthol AS-CA was changed to 178.9 parts of Naphthol AS-LC and 155.9 parts of Naphthol AS-KB, and 1639 parts of methanol was changed to 1311 parts of N-methyl-2-pyrrolidone and 420 parts of water. Except for these changes, 580.6 parts of Colorant 40 were obtained in the same manner as in Example 18.
[0221] (Examples 41 to 44) Production of Colorants 41 to 44 Colorants 40 to 44 were obtained in the same manner as in Example 18, except that 327.8 parts of naphthol AS-CA as the coupler component was changed to the corresponding first coupler type and parts by mass of the first coupler and second coupler type and parts by mass of the second coupler in Table 1.
[0222] Example 45: Production of Colorant 45 The base component was changed from 245.9 parts to 244.7 parts of 3-amino-4-methoxybenzanilide, 3643 parts of water was changed to a mixture of 1450 parts of acetonitrile and 2200 parts of water, 0.74 parts of 3-amino-4-methoxybenzanilide was added to the coupler solution, and the methanol used to dissolve the coupler was changed to the same amount of acetonitrile. Except for these changes, 578.3 parts of Colorant 45 were obtained in the same manner as in Example 18.
[0223] (Example 46) Production of Colorant 46
[0123] The same procedure as in Example 1 was repeated except that the base component was changed from 237.4 parts of 3-amino-4-methoxybenzanilide to 218 parts, and the amount of compound (B) added to the coupler component was changed to 1.1 parts, to obtain 496.3 parts of Colorant 46.
[0224] Examples 47 to 55 Production of Colorants 47 to 55 As the base component, 245.9 parts of 3-amino-4-methoxybenzanilide was changed to the corresponding base type and base parts by mass in Table 1, and as the coupler component, 327.8 parts by mass of naphthol AS-CA was changed to the corresponding first coupler type and first coupler parts by mass in Table 1, and further, the methanol used to dissolve the coupler was changed to the same amount of acetone. Except for this, Colorants 47 to 55 were obtained in the same manner as in Example 18.
[0225] Example 56: Production of Colorant 56 The base component was changed from 245.9 parts to 266.5 parts of 3-amino-4-methoxybenzanilide, the methanol used to dissolve the coupler was changed to a mixture of 820 parts of tetrahydrofuran and 820 parts of water, and 27.5 parts of 4MPB was added as compound (B) to the coupler solution. Except for these changes, colorant 56 was obtained in the same manner as in Example 18.
[0226] (Example 57) Preparation of Colorant 57 147.2 parts of 3-amino-4-methylbenzamide as the base component was added to 3,518 parts of water and stirred to prepare a suspension. 1,465 parts of ice was then added and the temperature was adjusted to 5°C or below. 389.0 parts of 35% hydrochloric acid was added thereto and stirred for 30 minutes. Subsequently, an aqueous solution prepared by adding 69.9 parts of sodium nitrite to 104.8 parts of water was added and stirred for 1 hour to carry out diazotization. Sulfamic acid was added to the reaction mixture obtained by the above diazotization, and excess nitrous acid was removed. Sulfamic acid was added until no free nitrous acid was detected using potassium iodide paper. 203.0 parts of sodium acetate and 22.4 parts of 80% acetic acid were added to the mixture to prepare a solution containing a diazonium salt.
[0227] Separately, a mixture of 1,700 parts of water and 199.0 parts of a 40% aqueous sodium hydroxide solution was adjusted to 15 to 25°C. 293.3 parts of naphthol AS-RL was added and dissolved therein as a coupler component. 0.2 parts of 4-methylbenzamide (manufactured by Wako Pure Chemical Industries, Ltd.) was further added as compound (B) to form a coupler solution. This solution was added over 20 minutes to a solution containing a diazonium salt adjusted to 25°C, and a coupling reaction was carried out.
[0228] The slurry obtained by the coupling reaction was stirred for 1 hour, then heated to 70°C and stirred at 68 to 72°C for an additional 1 hour. The pH at this time was 4.5. The slurry was cooled to 50°C or below, filtered, and washed with water to obtain a press cake of colorant. The press cake was dried at 80°C for 18 hours and then pulverized to obtain 436.7 parts of Colorant 57.
[0229] Examples 58 to 63 Production of Colorants 58 to 63 Colorants 58 to 63 were obtained in the same manner as in Example 1, except that 147.2 parts of 3-amino-4-methylbenzamide was used as the base component, the corresponding base type and base parts by mass in Table 1 was used, 293.3 parts of naphthol AS-RL was used as the coupler component, the corresponding first coupler type and first coupler parts by mass in Table 1 was used, and 0.2 parts by mass of compound (B) was changed to the corresponding type and part by mass of compound (B) in Table 1-7.
[0230] (Example 64) Preparation of Colorant 64 157.7 parts of 3-amino-4-methylbenzamide as the base component was added to 3,643 parts of water and stirred to prepare a suspension. 1,517 parts of ice was then added and the temperature was adjusted to 5°C or below. 402.9 parts of 35% hydrochloric acid was added thereto and stirred for 30 minutes. Subsequently, an aqueous solution prepared by adding 72.3 parts of sodium nitrite to 108.5 parts of water was added and stirred for 1 hour to carry out diazotization. Sulfamic acid was added to the reaction mixture to remove excess nitrous acid. Sulfamic acid was added until no free nitrous acid was detected using potassium iodide paper. 210.2 parts of sodium acetate and 23.2 parts of 80% acetic acid were added to the mixture to prepare a solution containing a diazonium salt.
[0231] Separately, a mixture of 1,670 parts of water and 199.0 parts of a 40% aqueous sodium hydroxide solution was adjusted to 15 to 25°C. 293.3 parts of Naphthol AS-RL was added and dissolved therein as a coupler component to prepare a coupler solution. This solution was added over 20 minutes to a solution containing a diazonium salt adjusted to 25°C, to carry out a coupling reaction.
[0232] The slurry obtained by the coupling reaction was stirred for 1 hour, then heated to 70°C and stirred at 68 to 72°C for an additional 1 hour. At this time, the pH was 4.5. The slurry was cooled to 50°C or below, filtered, and washed with water to obtain a press cake of colorant. The press cake was dried at 80°C for 18 hours and then pulverized to obtain 454.6 parts of Colorant 64.
[0233] Examples 65 to 70 Production of Colorants 65 to 70 Colorants 65 to 70 were obtained in the same manner as in Example 64, except that 157.7 parts of 3-amino-4-methylbenzamide as the base component was changed to the corresponding base type and base parts by mass in Table 1, and 293.3 parts of naphthol AS-RL as the coupler component was changed to the corresponding first coupler type and first coupler parts by mass in Table 1.
[0234] Comparative Examples 1 to 17: Production of Colorants 101 to 117 Colorants 101 to 117 were obtained in the same manner as in Examples 1 to 17, except that compound (B) was not added.
[0235] Comparative Examples 18 to 24: Production of Colorants 118 to 124 Colorants 118 to 124 were obtained in the same manner as in Examples 57 to 63, except that compound (B) was not added.
[0236] In Examples 1 to 70 and Comparative Examples 1 to 24, the raw materials used in the production of the colorants are summarized in Tables 1-1, 1-2 and 1-2A.
[0237]
[0238]
[0239]
[0240] Furthermore, for each of the colorants produced in Examples 1 to 70 and Comparative Examples 1 to 24, specific combinations of compound (A) and compound (B) are summarized in Tables 1-3 to 1-7 below.
[0241]
[0242]
[0243]
[0244]
[0245]
[0246] <2> Quantitative Analysis of Colorant The following describes the method for identifying and quantifying each component of the colorant. <Quantitative Analysis of Each Component: Compound (A)> Compound (A) contained in the colorants produced in Examples 1 to 70 and Comparative Examples 1 to 24 was quantitatively analyzed using absorptiometry according to the method described below. (Preparation of Standard Sample) 0.75 g of colorant, 30 ml of dimethyl sulfoxide, and 75 g of 0.3 mm zirconia beads were placed in a 50 ml glass bottle and dispersed for 2 hours at a vibration frequency of 172 rpm using a paint shaker (SK450 manufactured by Fast & Fluid), and the resulting dispersion was centrifuged for 30 minutes at a rotation speed of 9,500 rpm using a centrifuge Centrifuge 5810 (manufactured by Eppendorf). The residue after centrifugation was mixed with 30 ml of dimethyl sulfoxide and 0.1 g of 25% aqueous sodium hydroxide, stirred for 15 minutes, filtered, washed with water, dried at 80°C for 18 hours, and pulverized to obtain a standard colorant sample. (Measurement Sample Preparation) 40 mg of colorant was weighed into a 25 ml measuring flask, adjusted to volume with 0.1 g of 28% sodium methoxide in methanol and the remaining amount of dimethyl sulfoxide, and dissolved by shaking thoroughly. This solution was diluted 100 times by volume with dimethyl sulfoxide to obtain the measurement sample. (Measurement Method) The measurement sample was placed in a quartz cell with a 10 mm optical path length, and the absorbance was measured using a Hitachi UH4150 spectrophotometer. The absorbance per gram (absorbance / mass concentration) was calculated. The absorbance per gram was determined from the absorbance of the peak in the 400-700 nm range (548 nm for Pigment Red 269). Similarly, the extinction coefficient per gram of the standard sample was measured and calculated, and the content of compound (A) was determined by dividing the extinction coefficient per gram of the colorant by the extinction coefficient per gram of the standard sample of the colorant.
[0247] <Quantitative Analysis of Each Component: Compounds (B), (C), (D), and (E)> The components contained in the colorants produced in Examples 1 to 70 and Comparative Examples 1 to 24 were quantitatively analyzed using high-performance liquid chromatography according to the method described below. (Extraction Method) 0.75 g of colorant, 30 ml of dimethyl sulfoxide, and 75 g of 0.3 mm zirconia beads were placed in a 50 ml glass bottle and dispersed for 2 hours at 172 rpm using a paint shaker (SK450 manufactured by Fast & Fluid). The resulting dispersion was centrifuged for 30 minutes at 9,500 rpm using a Centrifuge 5810 (manufactured by Eppendorf). The supernatant after centrifugation was filtered through a 0.2 μm filter. The liquid thus obtained was used as a measurement sample.
[0248] (Analysis Method) The amounts of compound (B), compound (C), compound (D), and compound (E) in the measurement sample were quantitatively analyzed using liquid chromatography. Note that compound (C) in the colorant is a substance represented by the following chemical formula (9), and compound (B), compound (D), and compound (E) are as shown in Tables 2-1, 2-2, and 2-3.
[0249]
[0250] The liquid chromatography conditions were as follows. The same quantitative analysis was repeated twice, and the average value was calculated. The calculated values were then converted into the content of each compound in the colorant. (Conditions) Apparatus: High-performance liquid chromatography Waters 2695 (manufactured by Waters) Column: Symmetry C18 180 mm x 2.1 mm 5 μm (manufactured by Waters) Sample: 10 μL Detector: UV-vis (Compound (B): 310 nm, Compound (C): 502 nm, Compound (D): 310 nm, Compound (E): 350 nm) Eluent: The composition was as shown in Table 2A. (A) was a 1 g / L aqueous ammonium acetate solution, and (B) was acetonitrile. Temperature: 35°C Flow rate: 0.3 ml / min Preparation of calibration curve: A calibration curve was prepared from the results of similar quantification using the target compounds.
[0251]
[0252] The results of the quantitative analysis of the colorants performed as described above are shown in Tables 2-1, 2-2, and 2-3. The content of compound (A) is the content relative to the entire colorant, and the content of each of the other components is the content relative to the total mass of compound (A) in the colorant. When there are multiple applicable components, the total value is shown. Note that the colorants may contain moisture or other trace components in addition to the components shown in Tables 2-1, 2-2, and 2-3.
[0253]
[0254]
[0255]
[0256] In addition to the commercially available products described above, compounds synthesized by the following method were used as the compound (B) for quantification. (Production Example 1) Production of DA-R185: 7.4 parts of powdered sodium nitrite were added in small portions to 7.4 parts of 97% concentrated sulfuric acid at 0°C with gentle stirring. A solution of 6 parts of R185 base in 7.4 parts of 97% concentrated sulfuric acid was added dropwise while stirring. The reaction temperature was maintained at 5°C or below, and stirring was continued for 2 hours in an ice bath. Next, the reaction mixture was poured into a mixture containing 15 parts of hypophosphorous acid and 150 parts of ice with vigorous stirring. The mixture was stirred for 4 hours and then allowed to stand overnight at 20-25°C. The pH of the reaction mixture was adjusted to 8 by adding an ammonia solution, and then extracted three times with 50 parts of chloroform. The extract was dried over sodium sulfate, chromatographed on alumina, and the solvent was removed using a rotary evaporator to obtain 4.2 parts of DA-R185.
[0257] (Production Example 2) Production of DA-FVB DA-FVB was obtained in the same manner as in Production Example 1, except that 6 parts of R185 base in Production Example 1 was changed to 6.7 parts of Fast Violet B.
[0258] (Production Example 3) Production of DA-DC31 DA-DC31 was obtained in the same manner as in Production Example 1, except that 6 parts of R185 base in Production Example 1 was changed to 7.3 parts of Azoic DC31.
[0259] (Production Example 4) Production of DA-V32 DA-V32 was obtained in the same manner as in Production Example 1, except that 6 parts of the R185 base in Production Example 1 was changed to 6.5 parts of V32 base.
[0260] <3> Coloring Composition The following relates to specific examples of coloring compositions containing the colorants prepared above. Pigment Dispersion (A1) Preparation of Pigment Dispersion (Example A-1) Preparation of Pigment Dispersion a-1 The following raw materials and 70 parts of zirconia beads with a diameter of 1.25 mm were placed in a 70 ml glass bottle and dispersed for 60 minutes using a Red Devil paint shaker to obtain a dispersion: Colorant 1: 3.15 parts Polyester-modified acrylic acid polymer (manufactured by Allnex, ADDITOLXW6528): 5.25 parts Wetting agent (manufactured by Allnex, ADDITOLVXW6374): 0.95 parts Antifoaming agent (manufactured by Allnex, ADDITOLVXW6211): 0.63 parts Ion-exchanged water: 21.52 parts Next, the zirconia beads were removed from the dispersion to obtain Pigment Dispersion a-1.
[0261] (Examples A-2 to A-70, Comparative Examples A-1 to A-24) Preparation of Pigment Dispersions a-2 to a-70 and a-101 to a-124 Pigment dispersions a-2 to a-70 and a-101 to a-124 were obtained in the same manner as in Example A-1, except that colorant 1 in Example A-1 was changed as shown in Tables 3-1, 3-2, and 3-3.
[0262] (A2) Evaluation of Pigment Dispersion <Initial Viscosity and Viscosity Stability> The initial viscosity of the obtained pigment dispersion was measured at 25°C using an E-type viscometer ("ELD-type viscometer" manufactured by Toki Sangyo Co., Ltd.). Similarly, the viscosity after accelerated aging at 60°C for one week was measured. The viscosity increase rate relative to the initial viscosity was calculated based on the obtained measured value, and used as an index of viscosity stability, and evaluated according to the following evaluation criteria. The results are shown in Tables 3-1, 3-2, and 3-3. The lower the initial viscosity, the better the dispersibility. Furthermore, the smaller the viscosity increase rate, the better the dispersion stability. A rating of "4," "3," or "2" on the following evaluation criteria is at a practical level. Note that Tables 3-1, 3-2, and 3-3 show only compound (A), which is the main component of the colorant, but the details of each colorant are as shown above in Tables 2-1, 2-2, and 2-3.
[0263] (Evaluation criteria for initial viscosity) 4: The initial viscosity is less than 5.0 mPa·s. Very good 3: The initial viscosity is 5.0 mPa·s or more and less than 7.5 mPa·s. Good 2: The initial viscosity is 7.5 mPa·s or more and less than 10.0 mPa·s. Practical use is possible 1: The initial viscosity is 10.0 mPa·s or more. Poor
[0264] (Evaluation criteria for viscosity stability) 4: Viscosity increase rate is less than 20%. Very good 3: Viscosity increase rate is 20% or more and less than 30%. Good 2: Viscosity increase rate is 30% or more and less than 40%. Practical use possible 1: Viscosity increase rate is 40% or more. Poor
[0265]
[0266]
[0267]
[0268] Below, examples of coloring compositions are given of paints and printing inks constructed using the colorants or pigment dispersions prepared above. The hue of a colorant varies depending on its structure. Therefore, the evaluation of the coloring strength, vividness, and transparency of the colorants described below was performed using a pigment with the same C.I. No. as a comparison control. In each table, only the main component compound (A) (pigment) is shown for the colorant, but the details of each colorant are as shown in Tables 2-1, 2-2, and 2-3. The comparison control (standard) is indicated as "std." Furthermore, for pigments containing multiple C.I. Nos., C.I. Pigment Red 269 was used as the comparison control for all pigments.
[0269] Preparation of Water-Based Coating (B1) Water-Based Coating and Coating Film (Example B-1) Preparation of Water-Based Coating b-1 and Fabrication of Coating Film The following raw materials were stirred using a high-speed stirrer to obtain water-based coating b-1. Pigment dispersion a-1: 1.4 parts Acrylic resin (DIC Corporation, Burnock WD-304): 13.6 parts Melamine resin (Allnex Corporation, Cymel 325): 3.4 parts
[0270] The resulting aqueous paint b-1 was applied to a commercially available polyethylene terephthalate (PET) film with a thickness of 100 μm using a 7 mil applicator. After application, the PET film was dried at room temperature for 18 hours. Thereafter, it was dried at 60°C for 5 minutes and at 140°C for 20 minutes to obtain a coated film.
[0271] (Examples B-2 to B-70, Comparative Examples B-1 to B-24) Preparation of water-based paints b-2 to b-70, b-101 to b-124, and production of coating films Water-based paints b-2 to b-70, b-101 to b-124, and their coating films were obtained in the same manner as in Example B-1, except that the pigment dispersion 1 in Example B-1 was changed as shown in Tables 4-1, 4-2, and 4-3.
[0272] (B2) Evaluation of Paint Films <Tinting Strength> Films coated with paint (coated objects) were visually observed and evaluated according to the following criteria. The results are shown in Tables 4-1, 4-2, and 4-3. The reference coated object was a comparative example coated object in which a pigment with the same C.I. No. as the compound (A) in the adhesive used in the examples was used, as described above. In addition, when the colorant contained multiple compounds (A), the comparative example coated object in which all C.I. Pigment Red 269 was used was used as the control (reference). The same criteria were applied to clarity. (Evaluation criteria for tinting strength) 4: Tinting strength significantly higher than the reference coated object 3: Tinting strength higher than the reference coated object 2: Tinting strength slightly higher than the reference coated object 1: Tinting strength equivalent to the reference coated object
[0273] <Clarity> The coated films (coated objects) were visually observed and evaluated according to the following criteria. The results are shown in Tables 4-1, 4-2, and 4-3. The reference coated objects are as explained above. (Evaluation criteria for clarity) 4: Extremely higher clarity than the reference coated object 3: Higher clarity than the reference coated object 2: Slightly higher clarity than the reference coated object 1: Equivalent clarity to the reference coated object
[0274]
[0275]
[0276]
[0277] <C> Aqueous Inkjet Inks (C1) Preparation of Aqueous Inkjet Inks (Aqueous IJ Inks) (Example C-1) Preparation of Aqueous IJ Ink c-1 The following raw materials, colorant 1: 19.0 parts, styrene-acrylic acid copolymer (manufactured by BASF Japan Ltd., JONCRYL 61J): 16.4 parts, surfactant (manufactured by Kao Corporation, EMULGEN 420): 5.0 parts, and ion-exchanged water: 59.6 parts, and 200 parts of zirconia beads with a diameter of 1.25 mm, were placed in a 200 ml glass bottle and dispersed for 6 hours using a paint shaker manufactured by Red Devil Co., Ltd. Next, the zirconia beads were removed from the dispersion to obtain a pigment dispersion.
[0278] Next, the above pigment dispersion and the following raw materials were mixed and stirred for 30 minutes using a high-speed mixer to obtain a mixture: - Obtained pigment dispersion: 12.5 parts - Styrene-acrylic acid copolymer (Joncryl 60, manufactured by BASF Japan Ltd.): 3.3 parts - Surfactant (Emulgen 420, manufactured by Kao Corporation): 2.0 parts - Ion-exchanged water: 64.9 parts Next, diethylene glycol monobutyl ether was added appropriately to the above mixture to adjust the viscosity at 25°C to 2.5 mPa s (25°C) and the surface tension to 40 mN / m, and then the mixture was filtered using a 1.0 μm membrane filter and further filtered using a 0.45 μm membrane filter to obtain aqueous IJ ink c-1.
[0279] (Examples c-2 to c-70, Comparative Examples c-1 to c-24) Preparation of Water-Based IJ Inks c-2 to c-70, c-101 to c-124 Water-based IJ inks c-2 to c-70, c-101 to c-124 were obtained in the same manner as in Example C-1, except that colorant 1 in Example c-1 was changed as shown in Tables 5-1, 5-2, and 5-3.
[0280] (C2) Evaluation of Water-Based Inkjet Ink <Tinting Strength> The prepared water-based inkjet ink was filled into the cartridge of a Seiko Epson PX-105 printer (piezo inkjet printer), and printing was carried out on A4-sized plain paper. The printed matter was visually observed and evaluated according to the following criteria. The reference printed matter was as explained above. The results are shown in Tables 5-1, 5-2, and 5-3. (Evaluation criteria for tinting strength) 4: Tinting strength is extremely higher than the reference printed matter 3: Tinting strength is higher than the reference printed matter 2: Tinting strength is slightly higher than the reference printed matter 1: Tinting strength is equivalent to that of the reference printed matter
[0281] <Clarity> The printed matter used in the evaluation of coloring strength was visually observed and evaluated according to the following criteria. The reference printed matter was as explained above. The results are shown in Tables 5-1, 5-2, and 5-3. (Evaluation criteria for clarity) 4: Extremely higher clarity than the reference printed matter 3: Higher clarity than the reference printed matter 2: Slightly higher clarity than the reference printed matter 1: Equivalent clarity to the reference printed matter
[0282] <Transparency> The prepared aqueous inkjet ink was filled into the cartridge of a Seiko Epson printer HG-5130, and printing was carried out on a polyethylene terephthalate film attached to A4 plain paper. The print was placed on black construction paper, and the transparency of the black construction paper was visually observed and evaluated according to the following criteria. The reference print was as described above. The results are shown in Tables 5-1, 5-2, and 5-3. (Transparency evaluation criteria) 4: Extremely more transparent than the reference print 3: More transparent than the reference print 2: Slightly more transparent than the reference print 1: Equivalent transparency to the reference print
[0283] In addition, when the substrate was changed from A4-size plain paper to coated paper, polypropylene film (OPP film), or aluminum foil, and the coloring power was evaluated, similar results were obtained. When the substrate was not paper, the substrate was attached to A4-size plain paper. Furthermore, when a tank filled with the prepared aqueous inkjet ink was installed as a magenta ink in a Canon MAXIFYMB5430 (thermal inkjet printer), the coloring power was evaluated, and similar results were obtained.
[0284] <Viscosity Stability> The initial viscosity of each aqueous inkjet ink was measured at 25°C using an E-type viscometer ("ELD-type viscometer" manufactured by Toki Sangyo Co., Ltd.). In the same manner, the viscosity after accelerated aging at 70°C for 2 weeks was measured. Using each measured value, the viscosity increase rate relative to the initial viscosity was calculated, which was used as an index of viscosity stability and evaluated according to the following criteria. The results are shown in Tables 5-1, 5-2, and 5-3. The smaller the viscosity increase rate, the better the viscosity stability is considered to be, and a rating of "3" or "2" on the following evaluation criteria is at a practical level. (Evaluation criteria for viscosity stability) 3: Viscosity increase rate is less than 15% 2: Viscosity increase rate is 15% or more but less than 30% 1: Viscosity increase rate is 30% or more
[0285]
[0286]
[0287]
[0288] <D> Gravure Ink (D1) Preparation of Gravure Ink First, the measurement methods for the resin are described below. (Hydroxyl Value) Determined in accordance with JIS K0070. (Acid Value) Determined in accordance with JIS K0070. (Amine Value) The amine value was determined in accordance with JIS K0070, using the equivalent amount of potassium hydroxide (mg) required to neutralize the amino groups contained in 1 g of resin. 0.5 to 2 g of sample was precisely weighed out (sample nonvolatile content: S g). 50 mL of a 60 / 40 (mass ratio) mixed solution of methanol and methyl ethyl ketone was added to dissolve the precisely weighed sample. Bromophenol blue was added as an indicator to the resulting solution, and the resulting solution was titrated with 0.2 mol / L ethanolic hydrochloric acid solution (titer: f). The point at which the solution color changed from green to yellow was set as the endpoint, and the titer (A mL) at this point was used to calculate the amine value according to the following formula: Amine value = (A x f x 0.2 x 56.108) / S [mg KOH / g]
[0289] (Weight-average molecular weight) The weight-average molecular weight was determined by measuring the molecular weight distribution using a GPC (gel permeation chromatography) device (HLC-8220 manufactured by Tosoh Corporation) and calculating the molecular weight as a converted value using polystyrene as a standard substance. The measurement conditions are shown below. Column: The following columns were connected in series and used. Guard column HXL-H manufactured by Tosoh Corporation TSKgel G5000HXL manufactured by Tosoh Corporation TSKgel G4000HXL manufactured by Tosoh Corporation TSKgel G3000HXL manufactured by Tosoh Corporation TSKgel G2000HXL manufactured by Tosoh Corporation Detector: RI (differential refractometer) Measurement conditions: Column temperature 40°C Eluent: tetrahydrofuran Flow rate: 1.0 mL / min
[0290] (Glass Transition Temperature) The glass transition temperature (Tg) was determined by DSC (differential scanning calorimetry) using a Rigaku DSC8231 measuring instrument, with a measurement temperature range of −70 to 250° C., a temperature rise rate of 10° C. / min, and the midpoint between the endothermic start and end temperatures due to the glass transition in the DSC curve being taken as the glass transition temperature.
[0291] (Synthesis Example 1) [Polyurethane Resin PU1] 200 parts of polypropylene glycol (hereinafter "PPG700") having a number average molecular weight (Mn) of 700, 127 parts of isophorone diisocyanate (hereinafter "IPDI"), and 81.8 parts of ethyl acetate were reacted under a nitrogen stream at 80°C for 4 hours to obtain a resin solution of isocyanate-terminated urethane prepolymer. Next, 49.5 parts of isophorone diamine (hereinafter "IPDA"), 3 parts of 2-ethanolamine, and 803.9 parts of a 50 / 50 (mass ratio) ethyl acetate / isopropanol (hereinafter "IPA") mixed solvent were added slowly to the obtained resin solution of isocyanate-terminated urethane prepolymer at 40°C, and the mixture was allowed to react for 1 hour at 80°C to obtain a polyurethane resin solution PU1 having a nonvolatile content of 30%, an amine value of 3.5 mg KOH / g, a hydroxyl value of 7.3 mg KOH / g, and a weight average molecular weight of 40,000. The glass transition temperature was -32°C.
[0292] Example D-1 Preparation of Gravure Ink d-1 30 parts of polyurethane resin solution PU1 (non-volatile content 30%) as a resin, 0.8 parts in terms of non-volatile content of polyethylene wax (Honeywell A-C400A) as a hydrocarbon wax, 0.5 parts in terms of non-volatile content of chlorinated polypropylene resin (Nippon Paper Industries Co., Ltd. 370M chlorine content 30% non-volatile content 50%), 10 parts of Colorant 1, and 58.7 parts of a solution of methyl ethyl ketone (hereinafter referred to as "MEK") / n-propyl acetate (hereinafter referred to as "NPAC") / IPA = 40 / 40 / 20 (mass ratio) were mixed and dispersed for 15 minutes using an Eiger mill to obtain gravure ink d-1.
[0293] (Examples D-2 to D-70, Comparative Examples D-1 to D-24) Preparation of Gravure Inks d-2 to d-70 and d-101 to d-124 Gravure inks d-2 to d-70 and d-101 to d-124 were obtained in the same manner as in Example D-1, except that colorant 1 in Example D-1 was changed as shown in Tables 6-1, 6-2, and 6-3.
[0294] (D2) Preparation of Gravure Ink Prints The gravure ink obtained above was diluted with a mixed solvent consisting of MEK / NPAC / IPA = 40 / 40 / 20 (mass ratio) to a viscosity of 16 seconds (25°C, Zahn cup No. 3), and printed on the following substrates (corona discharge treated surface in the case of OPP) at a printing speed of 80 m / min using a gravure printing machine equipped with a Helio 175 line gradation plate (plate type compressed gradation 100% to 3%) to obtain OPP prints and CPP prints. (Substrates) OPP: biaxially oriented polypropylene (OPP) film with corona discharge treatment on one side (FOR manufactured by Futamura Chemical Co., Ltd., thickness 25 μm) CPP: unstretched polypropylene (CPP) film without corona treatment (CP-S manufactured by Mitsui Chemicals Tohcello, thickness 30 μm)
[0295] (D3) Evaluation of Gravure Ink and Printed Matter <Stability of Ink Over Time> Each of the prepared gravure inks was placed in a sealed container and stored at 40°C for 10 days. Thereafter, the viscosity was measured and the change in viscosity from before storage was evaluated. The viscosity was measured at 25°C using a Zahn cup No. 4 in seconds. The results are shown in Tables 6-1, 6-2, and 6-3. The viscosity of each ink measured with a Brookfield viscometer before storage was within the range of 40 to 500 cps (25°C). Evaluation results of "4," "3," and "2" according to the following evaluation criteria indicate a practical level. (Evaluation Criteria) 4: Viscosity change of less than 2 seconds (very good) 3: Viscosity change of 2 to less than 5 seconds (good) 2: Viscosity change of 5 to less than 10 seconds (practical) 1: Viscosity change of 10 seconds or more (poor)
[0296] <Clarity> The obtained OPP prints were visually observed and evaluated according to the following criteria. The results are shown in Tables 6-1, 6-2, and 6-3. Details of the standard prints (std) are as explained above. (Evaluation criteria for clarity) 4: Extremely clearer than the standard print 3: Clearer than the standard print 2: Slightly clearer than the standard print 1: Clearer than the standard print
[0297] <Transparency> The obtained OPP prints were visually observed and evaluated according to the following criteria. The results are shown in Tables 6-1, 6-2, and 6-3. Details of the standard prints (std) are as explained above. (Transparency evaluation criteria) 4: Extremely higher transparency than the standard print 3: Higher transparency than the standard print 3: Slightly higher transparency than the standard print 1: Equivalent transparency to the standard print
[0298] <Glossiness> The obtained OPP prints were visually observed and evaluated according to the following criteria. The results are shown in Tables 6-1, 6-2, and 6-3. Details of the standard prints (std) are as explained above. (Glossiness evaluation criteria) 4: Extremely higher gloss than the standard print 3: Higher gloss than the standard print 2: Equivalent gloss to the standard print 1: Lower gloss than the standard print
[0299]
[0300]
[0301]
[0302] <E> Active Energy Ray-Curable Flexographic Ink (E1) Preparation of Active Energy Ray-Curable Flexographic Ink (Example E-1) Preparation of Active Energy Ray-Curable Flexographic Ink e-1 The following materials were stirred and mixed using a butterfly mixer, and dispersed using a three-roll mill so that the maximum particle size would be 15 μm or less, to obtain active energy ray-curable flexographic ink e-1. Colorant 1: 18.0 parts EBECRYL 225: 8.4 parts (5.0 parts as active ingredient) (10-functional urethane acrylate oligomer) 4-acryloylmorpholine: 15.0 parts (monofunctional monomer) EO-modified trimethylolpropane triacrylate: 20.0 parts Dipentaerythritol pentaacrylate: 5.0 parts Dipentaerythritol hexaacrylate: 16.6 parts Irgacure 369: 3.0 parts (photopolymerization initiator) Chemrk DEABP: 3.0 parts (photopolymerization initiator) SB-PI718: 4.0 parts (photopolymerization initiator) AJISPER PB821: 3.0 parts (dispersant) T wax compound: 4.0 parts (wax)
[0303] Details of the materials used are as follows. [Acrylate oligomer] EBECRYL225: 10-functional aliphatic urethane acrylate oligomer, Mw 1,200, active ingredient 60% by mass, manufactured by Daicel Allnex Corporation [Polymerization initiator] Irgacure 369: 2-benzyl-2-(dimethylamino)-1-(4-morpholinophenyl)-1-butanone, manufactured by BASF Corporation Chemrk DEABP: 4,4'-bis(diethylamino)benzophenone, manufactured by Sort Corporation SB-PI718: 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, manufactured by Sort Corporation [Dispersant] AJISPER PB821: Comb-shaped dispersant containing basic functional groups, manufactured by Ajinomoto Fine-Techno Co., Ltd. [Wax] T Wax Compound: Polyethylene wax, manufactured by Toshin Yushi Co., Ltd.
[0304] (Examples e-2 to e-70, Comparative Examples e-1 to e-24) Preparation of active energy ray-curable flexographic inks e-2 to e-70 and e-101 to e-124 Except for changing colorant 1 in Example E-1 as shown in Tables 7-1, 7-2, and 7-3, the same procedure as in Example e-1 was carried out to obtain active energy ray-curable flexographic inks e-2 to e-70 and e-101 to e-124.
[0305] (E2) Evaluation of printed matter - Printing evaluation: Coated paper, line count 800 lpi, cell volume 3.72 cm 3 / m 2 After printing the ink using an anilox roller and a Flexiproof machine, the conveyor speed was 50 m / min and the ink was irradiated with an air-cooled mercury lamp (output 160 W / cm 2 The resulting mixture was cured under the conditions (conditions 1-3) to obtain a printed material for evaluation.
[0306] <Coloring strength> The printed matter was visually observed and evaluated according to the following criteria. The results are shown in Tables 7-1, 7-2, and 7-3. Details of the standard printed matter (std) are as explained above. (Evaluation criteria for coloring strength) 4: Coloring strength is much higher than the standard printed matter 3: Coloring strength is higher than the standard printed matter 2: Coloring strength is slightly higher than the standard printed matter 1: Coloring strength is the same as the standard printed matter
[0307] <Clarity> The prints were visually observed and evaluated according to the following criteria. The results are shown in Tables 7-1, 7-2, and 7-3. Details of the standard prints (std) are as explained above. (Evaluation criteria for clarity) 4: Extremely clearer than the standard print 3: Clearer than the standard print 2: Slightly clearer than the standard print 1: Clearer than the standard print
[0308] - Evaluation of printing on film Similarly, the ink was printed and cured on a corona-treated stretched polypropylene (OPP) film (Pylen P2161, manufactured by Toyobo Co., Ltd., thickness 40 μm) to obtain a printed film (printed material) for evaluation.
[0309] <Transparency> The obtained OPP prints were visually observed and evaluated according to the following criteria. The results are shown in Tables 7-1, 7-2, and 7-3. Details of the standard prints (std) are as explained above. (Evaluation criteria) 4: Extremely higher transparency than the standard print 3: Higher transparency than the standard print 2: Slightly higher transparency than the standard print 1: Equivalent transparency to the standard print
[0310] <Storage stability> 200 g of each ink was stored in a metal can at 25°C, and the condition of the ink after 6 months was evaluated. The results are shown in Tables 7-1, 7-2, and 7-3. (Evaluation criteria) 3: No increase in ink viscosity observed 2: Some increase in viscosity observed 1: Gelation or precipitation of raw materials observed
[0311]
[0312]
[0313]
[0314] <F> Active Energy Ray-Curable Offset Ink (F1) Preparation of Ink <Preparation of Resin Varnish> Prior to producing the active energy ray-curable ink, a resin varnish was prepared. The resin varnish was prepared by charging diallyl phthalate resin (Daiso DAP A (manufactured by Daiso Co., Ltd.)) / ditrimethylolpropane tetraacrylate / hydroquinone in a ratio of 30 / 69.9 / 0.1 and dissolving the mixture at 100°C under an air stream. <Preparation of Ink Compositions> (Example F-1) Preparation of Active Energy Ray-Curable Flexographic Ink f-1 25.8 parts of the above Colorant 1, 97.4 parts of the above Resin Varnish, 21.1 parts of ditrimethylolpropane tetraacrylate, 20 parts of dipentaerythritol hexaacrylate, 6 parts of magnesium carbonate, and 22.4 parts of a photopolymerization initiator were stirred and mixed using a butterfly mixer, and the mixture was dispersed using a three-roll mill so that the maximum particle size was 7.5 μm or less. Thereafter, the tack was adjusted to 7.5 to 8.0 with ditrimethylolpropane tetraacrylate, to prepare Active Energy Ray-Curable Offset Ink f-1.
[0315] (Examples F-2 to F-70, Comparative Examples F-1 to F-24) Preparation of active energy ray-curable offset inks f-2 to f-70 and f-101 to f-124 Except for changing colorant 1 in Example F-1 as shown in Tables 8-1, 8-2, and 8-3, the same procedure as in Example F-1 was carried out to obtain active energy ray-curable offset inks f-2 to f-70 and f-101 to f-124.
[0316] (F2) Various Evaluations and Printing Evaluation 0.4 ml of each of the obtained active energy ray curable offset inks was applied to an RI tester and spread evenly. Then, the ink was applied to Maricoat paper (coated cardboard manufactured by Hokuetsu Kishu Paper Co., Ltd.) and printed using a metal halide lamp (manufactured by Eye Graphics Co., Ltd.) irradiation device with an irradiation output of 96 W / cm. 2 The colored product was obtained by irradiating the product with ultraviolet light under the conditions of an irradiation distance of 10 mm and a conveyor speed of 50 m / min.
[0317] <Tinting strength> The printed matter was visually observed and evaluated according to the following criteria. The results are shown in Tables 8-1, 8-2, and 8-3. Details of the standard printed matter (std) are as explained above. (Evaluation criteria for tinting strength) 4: Tinting strength is much higher than the standard printed matter 3: Tinting strength is higher than the standard printed matter 2: Tinting strength is slightly higher than the standard printed matter 1: Tinting strength is the same as the standard printed matter
[0318] <Clarity> The prints were visually observed and evaluated according to the following criteria. The results are shown in Tables 8-1, 8-2, and 8-3. Details of the standard prints (std) are as explained above. (Evaluation criteria for clarity) 4: Extremely clearer than the standard print 3: Clearer than the standard print 2: Slightly clearer than the standard print 1: Clearer than the standard print
[0319] - Evaluation of printing on film Similarly, the ink was printed on a corona-treated oriented polypropylene (OPP) film (Pylen P2161, manufactured by Toyobo Co., Ltd., thickness 40 μm) and cured to obtain a printed film for evaluation.
[0320] <Transparency> The obtained OPP prints were visually observed and evaluated according to the following criteria. The results are shown in Tables 8-1, 8-2, and 8-3. Details of the standard prints (std) are as explained above. (Transparency evaluation criteria) 4: Extremely higher transparency than the standard print 3: Higher transparency than the standard print 2: Slightly higher transparency than the standard print 1: Equivalent transparency to the standard print
[0321] <Storage stability> 200g of each ink was stored in a metal can at 25°C and the condition of the ink after 6 months was evaluated. The results are shown in Tables 8-1, 8-2 and 8-3. (Evaluation criteria) 3: No increase in ink viscosity observed 2: Some increase in viscosity observed 1: Gelation or precipitation of raw materials observed
[0322]
[0323]
[0324]
[0325] <G> Molding Resin Composition (G1) Preparation of Molding Resin Composition (Example G-1) Preparation of Molding Resin Composition g-1 and Molded Product g'-1 2 parts of colorant 1 and 1,000 parts of polypropylene resin (product name: Prime Polypro J105, manufactured by Prime Polymer Co., Ltd.) were melt-kneaded at 220°C in a twin-screw extruder, and then cut with a pelletizer to obtain pelletized molding resin composition g-1. Next, this molding resin composition was injection molded using an injection molding machine to obtain a 1 mm thick molded product g'-1 (plate). The injection conditions were set at a molding temperature of 220°C and a mold temperature of 40°C.
[0326] (Examples g-2 to g-70, Comparative Examples g-1 to g-24) Preparation of molding resin compositions g-2 to g-70, g-101 to g-124 and molded bodies g'-2 to g'-70, g'-101 to g'-124 Except for changing colorant 1 in Example g-1 as shown in Tables 9-1, 9-2, and 9-3, the same procedures as in Example g-1 were carried out to obtain molding resin compositions g-2 to g-70, g-101 to g-124, and molded bodies g'-2 to g'-70, g'-101 to g'-124.
[0327] (G2) Evaluation of Molded Products <Dispersibility> Each of the produced molded products was visually observed to check for the presence or absence of coarse particles. The results are shown in Tables 9-1, 9-2 and 9-3.
[0328] <Clarity> Each produced molded body was visually observed and evaluated according to the following criteria. The results are shown in Tables 9-1, 9-2, and 9-3. Details of the standard molded body (std) are as explained above. (Evaluation criteria for clarity) 4: Much higher clarity than the standard molded body 3: Higher clarity than the standard molded body 2: Slightly higher clarity than the standard molded body 1: Equivalent clarity to the standard molded body
[0329]
[0330]
[0331]
[0332] <H> Toner (H1) Preparation of Negatively Charged Toner (Example H-1) Preparation of Negatively Charged Toner h-1 2500 parts of the obtained colorant 18 and 2500 parts of polyester resin (product name: M-325, manufactured by Sanyo Chemical Industries, Ltd.) were mixed and kneaded in a pressure kneader. The mixing and kneading were carried out at a set temperature of 120°C for 15 minutes. The obtained kneaded product was then removed from the pressure kneader and further kneaded using a three-roll mill at a roll temperature of 95°C. The obtained kneaded product was cooled and then coarsely pulverized to 10 mm or less to obtain a colored composition. 500 parts of the obtained coloring composition, 4375 parts of the polyester resin, 50 parts of a calcium salt compound of 3,5-di-tert-butylsalicylic acid (charge control agent), and 75 parts of an ethylene homopolymer (release agent, weight average molecular weight 850, Mw / Mn = 1.08, melting point 107°C) were mixed using a 20 L Henschel mixer (3000 rpm, 3 minutes), and further melt-kneaded using a twin-screw kneading extruder at a discharge temperature of 120°C. The kneaded mixture was then cooled and solidified, and then coarsely pulverized using a hammer mill. The resulting coarsely pulverized mixture was then finely pulverized using a Type I jet mill (IDS-2) and classified to obtain toner base particles. 2500 parts of the obtained toner base particles and 12.5 parts of hydrophobic titanium oxide (STT-30A, manufactured by Titan Kogyo Co., Ltd.) were mixed in a 10 L Henschel mixer to obtain negatively charged toner h-1.
[0333] Comparative Example H-1 Preparation of Negatively Charged Toner h-101 On the other hand, for comparison, negatively charged toner h-101 was obtained in the same manner as in Example H-1, except that Colorant 18 was changed to Colorant 101.
[0334] (H2) Evaluation of Negatively Charged Toners The obtained negatively charged toner h-1 and negatively charged toner h-101 were each sliced to a thickness of 0.9 μm using a microtome to form samples. Next, the dispersion state of the colorant in each sample was observed using a transmission electron microscope. As a result, it was found that the colorant was more uniformly distributed and more dispersible in the negatively charged toner h-1 using colorant 18 than in the negatively charged toner h-101 using colorant 101.
[0335] From the above results, it can be seen that a colorant containing compound (A) and compound (B) according to the present invention can improve the coloring strength, transparency, and clarity of conventional pigments. A resin composition containing a colorant according to the present invention can be suitably used in a variety of applications and can improve various properties. For example, in the form of an aqueous pigment dispersion, the initial viscosity and storage stability can be easily improved. In particular, in the form of an aqueous inkjet ink, excellent coloring strength, transparency, and clarity as well as excellent viscosity stability can be easily obtained. In particular, when the colorant contains two types of compound (A), even better clarity can be easily obtained.
Claims
1. A colorant comprising a compound (A) represented by the following general formula (1) and a compound (B) represented by the following general formula (2): [In the general formula (1) and the general formula (2), R 1 ~R 5 and R 1 '~R 5 each ' is independently a hydrogen atom, an alkoxy group, an alkyl group, a halogen group, a nitro group, a carboxy group, a sulfo group, a phosphate group, a sulfamoyl group, a carbamoyl group, a benzamido group, an alkylsulfamoyl group, an alkylcarbamoyl group, a group represented by the following general formula (101), a group represented by the following general formula (102), or a group represented by the following chemical formula (103), R 1 ~R 5 cannot all be hydrogen atoms at the same time, and R 1 '~R 5 ' cannot all be hydrogen atoms at the same time, 6 ~R 11 are each independently a hydrogen atom, an alkoxy group, an alkyl group, a halogen group, a nitro group, a carboxy group, a sulfo group, a phosphate group, a sulfamoyl group, a carbamoyl group, an alkylsulfamoyl group, an alkylcarbamoyl group, a group represented by the following general formula (104), or a group represented by the following general formula (105), R 6 ~R 11 are not all hydrogen atoms at the same time, and X is a hydrogen atom, a hydroxyl group, or a chlorine atom. [In the general formula (101), R 21 ~R 25 are each independently a hydrogen atom, an alkoxy group, an alkyl group, a halogen group, a nitro group, a carboxy group, a sulfo group, a phosphate group, a sulfamoyl group, a carbamoyl group, an alkylsulfamoyl group, an alkylcarbamoyl group, or an aryl group which may have a substituent, or R 21 ~R 25 Among these, two adjacent groups may be joined together to form a saturated or unsaturated alkylene group, or a saturated or unsaturated heteroalkylene group containing one or more heteroatoms selected from the group consisting of oxygen atoms, nitrogen atoms, and sulfur atoms, or a divalent group having a skeleton composed of a nitrogen atom and a carbonyl group, and the two adjacent groups may be joined together with the carbon atoms to which they are bonded to form a ring. [In the general formula (102), R 26 ~R 30 are each independently a hydrogen atom, an alkoxy group, an alkyl group, a halogen group, a nitro group, a carboxy group, a sulfo group, a phosphate group, a sulfamoyl group, a carbamoyl group, an alkylsulfamoyl group, an alkylcarbamoyl group, or an aryl group which may have a substituent, or R 26 ~R 30 Among these, two adjacent groups may be joined together to form a saturated or unsaturated alkylene group, or a saturated or unsaturated heteroalkylene group containing one or more heteroatoms selected from the group consisting of oxygen atoms, nitrogen atoms, and sulfur atoms, or a divalent group having a skeleton composed of a nitrogen atom and a carbonyl group, and the two adjacent groups may be joined together with the carbon atoms to which they are bonded to form a ring. [In the general formula (104), R 31 ~R 35 are each independently a hydrogen atom, an alkoxy group, an alkyl group, a halogen group, a nitro group, a carboxy group, a sulfo group, a phosphate group, a sulfamoyl group, a carbamoyl group, an alkylsulfamoyl group, an alkylcarbamoyl group, or an aryl group which may have a substituent, or R 31 ~R 35 Among these, two adjacent groups may be joined together to form a saturated or unsaturated alkylene group, or a saturated or unsaturated heteroalkylene group containing one or more heteroatoms selected from the group consisting of oxygen atoms, nitrogen atoms, and sulfur atoms, or a divalent group having a skeleton composed of a nitrogen atom and a carbonyl group, and the two adjacent groups may be joined together with the carbon atoms to which they are bonded to form a ring. [In the general formula (105), R 36 ~R 40 are each independently a hydrogen atom, an alkoxy group, an alkyl group, a halogen group, a nitro group, a carboxy group, a sulfo group, a phosphate group, a sulfamoyl group, a carbamoyl group, an alkylsulfamoyl group, an alkylcarbamoyl group, or an aryl group which may have a substituent, or R 36 ~R 40 Among these, two adjacent groups may be joined together to form a saturated or unsaturated alkylene group, or a saturated or unsaturated heteroalkylene group containing one or more heteroatoms selected from the group consisting of oxygen atoms, nitrogen atoms, and sulfur atoms, or a divalent group having a skeleton composed of a nitrogen atom and a carbonyl group, and the two adjacent groups may be joined together with the carbon atoms to which they are bonded to form a ring.
2. The colorant according to claim 1, wherein X in said general formula (2) is a hydrogen atom.
3. In the general formula (1) and the general formula (2), R 1 ~R 5 and R 1 '~R 5 R ′ each independently represents a hydrogen atom, an alkoxy group, an alkyl group, a nitro group, a carboxy group, a carbamoyl group, a benzamide group, an alkylsulfamoyl group, a group represented by the general formula (101) or a group represented by the chemical formula (103), 6 ~R 11 each independently represents a hydrogen atom, a carbamoyl group, or a group represented by general formula (104), 4. The colorant according to any one of claims 1 to 3, wherein the compound (A) includes a compound represented by the following general formula (3), and the compound (B) includes a compound represented by the following general formula (4): [In the general formula (3), R 6 ~R 11 are each independently a hydrogen atom, an alkoxy group, an alkyl group, a halogen group, a nitro group, a carboxy group, a sulfo group, a phosphate group, a sulfamoyl group, a carbamoyl group, an alkylsulfamoyl group, an alkylcarbamoyl group, a group represented by general formula (104), or a group represented by general formula (105), R 6 ~R 11 cannot all be hydrogen atoms at the same time. [In general formula (4), X is a hydrogen atom, a hydroxyl group, or a chlorine atom.] 5. The colorant according to any one of claims 1 to 4, wherein the compound (A) comprises one or more selected from the group consisting of C. I. Pigment Red 17, 22, 23, 31, 32, 114, 146, 147, 150, 176, 185, 245, 258, 268, and 269, and C. I. Pigment Violet 32 and 50.
6. The colorant according to any one of claims 1 to 5, wherein the content of said compound (B) relative to the total mass of said compound (A) is 0.01 mass % or more and 10 mass % or less.
7. The colorant according to any one of claims 1 to 6, further comprising at least one selected from the group consisting of compound (C) represented by the following general formula (5), compound (D) represented by the following general formula (6), and compound (E) represented by the following general formula (7), and satisfying any one of the following requirements (i) to (iii): (i) the content of compound (C) relative to the total mass of compound (A) is 0.001% by mass or more and 0.5% by mass or less, (ii) the content of compound (D) relative to the total mass of compound (A) is 0.12% by mass or less, and (iii) the content of compound (E) relative to the total mass of compound (A) is 6% by mass or less. [In the general formula (5), R 1 ~R 5 are each independently a hydrogen atom, an alkoxy group, an alkyl group, a halogen group, a nitro group, a carboxy group, a sulfo group, a phosphate group, a sulfamoyl group, a carbamoyl group, an alkylsulfamoyl group, an alkylcarbamoyl group, a group represented by the general formula (101), a group represented by the general formula (102), or a group represented by the chemical formula (103), R 1 ~R 5 cannot all be hydrogen atoms at the same time. [In the general formula (6), R 1 '~R 5 each ' is independently a hydrogen atom, an alkoxy group, an alkyl group, a halogen group, a nitro group, a carboxy group, a sulfo group, a phosphate group, a sulfamoyl group, a carbamoyl group, an alkylsulfamoyl group, an alkylcarbamoyl group, a group represented by the general formula (101), a group represented by the general formula (102), or a group represented by the chemical formula (103), R 1 '~R 5 ' cannot all be hydrogen atoms at the same time. [In the general formula (7), R 6 ~R 11 are each independently a hydrogen atom, an alkoxy group, an alkyl group, a halogen group, a nitro group, a carboxy group, a sulfo group, a phosphate group, a sulfamoyl group, a carbamoyl group, an alkylsulfamoyl group, an alkylcarbamoyl group, a group represented by the general formula (104) or a group represented by the general formula (105), R 6 ~R 11 cannot all be hydrogen atoms at the same time.
8. A coloring composition comprising the colorant according to any one of claims 1 to 7 and a dispersion medium.
9. A printing ink comprising the colorant according to any one of claims 1 to 7, a resin, and a solvent.
10. An active energy ray-curable printing ink comprising the colorant according to any one of claims 1 to 7 and a polymerizable compound.
11. A method for producing a colorant containing a compound (A) represented by the following general formula (1) and a compound (B) represented by the following general formula (2), comprising carrying out a coupling reaction between a solution containing a coupler component represented by the following general formula (7) and a solution containing a diazonium salt represented by the following general formula (6A) obtained by diazotizing an aromatic amine, using an excess amount of diazonium salt in terms of a molar ratio relative to the coupler component. [In the general formula (1) and the general formula (2), R 1 ~R 5 and R 1 '~R 5 each ' is independently a hydrogen atom, an alkoxy group, an alkyl group, a halogen group, a nitro group, a carboxy group, a sulfo group, a phosphate group, a sulfamoyl group, a carbamoyl group, a benzamido group, an alkylsulfamoyl group, an alkylcarbamoyl group, a group represented by the following general formula (101), a group represented by the following general formula (102), or a group represented by the following chemical formula (103), R 1 ~R 5 are not all hydrogen atoms at the same time, and R 1 '~R 5 ' cannot all be hydrogen atoms at the same time, 1 ~R 5 and the corresponding R 1 '~R 5 R ′ are the same groups as each other, 6 ~R 11 are each independently a hydrogen atom, an alkoxy group, an alkyl group, a halogen group, a nitro group, a carboxy group, a sulfo group, a phosphate group, a sulfamoyl group, a carbamoyl group, an alkylsulfamoyl group, an alkylcarbamoyl group, a group represented by the following general formula (104), or a group represented by the following general formula (105), R 6 ~R 11 are not all hydrogen atoms at the same time, and X is a hydrogen atom, a hydroxyl group, or a chlorine atom. [In the general formula (101), R 21 ~R 25 are each independently a hydrogen atom, an alkoxy group, an alkyl group, a halogen group, a nitro group, a carboxy group, a sulfo group, a phosphate group, a sulfamoyl group, a carbamoyl group, an alkylsulfamoyl group, an alkylcarbamoyl group, or an aryl group which may have a substituent, or R 21 ~R 25 Among these, two adjacent groups may be joined together to form a saturated or unsaturated alkylene group, or a saturated or unsaturated heteroalkylene group containing one or more heteroatoms selected from the group consisting of oxygen atoms, nitrogen atoms, and sulfur atoms, or a divalent group having a skeleton composed of a nitrogen atom and a carbonyl group, and the two adjacent groups may be joined together with the carbon atoms to which they are bonded to form a ring. [In the general formula (102), R 26 ~R 30 are each independently a hydrogen atom, an alkoxy group, an alkyl group, a halogen group, a nitro group, a carboxy group, a sulfo group, a phosphate group, a sulfamoyl group, a carbamoyl group, an alkylsulfamoyl group, an alkylcarbamoyl group, or an aryl group which may have a substituent, or R 26 ~R 30 Among these, two adjacent groups may be joined together to form a saturated or unsaturated alkylene group, or a saturated or unsaturated heteroalkylene group containing one or more heteroatoms selected from the group consisting of oxygen atoms, nitrogen atoms, and sulfur atoms, or a divalent group having a skeleton composed of a nitrogen atom and a carbonyl group, and the two adjacent groups may be joined together with the carbon atoms to which they are bonded to form a ring. [In the general formula (104), R 31 ~R 35 are each independently a hydrogen atom, an alkoxy group, an alkyl group, a halogen group, a nitro group, a carboxy group, a sulfo group, a phosphate group, a sulfamoyl group, a carbamoyl group, an alkylsulfamoyl group, an alkylcarbamoyl group, or an aryl group which may have a substituent, or R 31 ~R 35 Among these, two adjacent groups may be joined together to form a saturated or unsaturated alkylene group, or a saturated or unsaturated heteroalkylene group containing one or more heteroatoms selected from the group consisting of oxygen atoms, nitrogen atoms, and sulfur atoms, or a divalent group having a skeleton composed of a nitrogen atom and a carbonyl group, and the two adjacent groups may be joined together with the carbon atoms to which they are bonded to form a ring. [In the general formula (105), R 36 ~R 40 are each independently a hydrogen atom, an alkoxy group, an alkyl group, a halogen group, a nitro group, a carboxy group, a sulfo group, a phosphate group, a sulfamoyl group, a carbamoyl group, an alkylsulfamoyl group, an alkylcarbamoyl group, or an aryl group which may have a substituent, or R 36 ~R 40 Among these, two adjacent groups may be joined together to form a saturated or unsaturated alkylene group, or a saturated or unsaturated heteroalkylene group containing one or more heteroatoms selected from the group consisting of oxygen atoms, nitrogen atoms, and sulfur atoms, or a divalent group having a skeleton composed of a nitrogen atom and a carbonyl group, and the two adjacent groups may be joined together with the carbon atoms to which they are bonded to form a ring. [In the general formula (7), R 6 ~R 11 is R in the general formula (1). 6 ~R 11 is the same as: [In the general formula (6A), R 1 ~R 5 is R in the general formula (1) 1 ~R 5 is the same as:
Citation Information
Patent Citations
Monoazo-based red pigment composition and magenta color toner
JP2000248191A
Magenta toner and method for forming image
JP2003149869A
Capsid inhibitors for the treatment of HIV
JP2023054361A
Nano-scale pigment particle composition
JP2011026601A
Colored film set for color filter
JP2013148855A