Resin sheet, heat dissipation member, laminate, resin composition, cured article, circuit board, and semiconductor chip package
The resin sheet with a high volume of monocrystalline fillers and a mesogenic epoxy resin, combined with a cyanate ester curing agent, addresses the challenges of thermal conductivity and filler separation in miniaturized electronic devices, enhancing both performance and manufacturing simplicity.
Patent Information
- Application Number
- PCT/JP2024/012962
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-09-21
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional heat dissipating insulating resin sheets face challenges in maintaining thermal conductivity while preventing resin and filler separation, especially in miniaturized electronic devices with narrow gaps, and in improving flexibility without complicating the manufacturing process.
A resin sheet with a thermally conductive filler content of 50-80% by volume, featuring monocrystalline fillers and an epoxy resin with a mesogenic skeleton, along with a cyanate ester curing agent, is used to enhance thermal conductivity and flexibility without filler separation.
The solution effectively improves thermal conductivity and flexibility of the resin sheet, preventing filler separation and ensuring reliable heat dissipation in miniaturized devices without complicating the manufacturing process.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Resin sheet, heat dissipation member, laminate, resin composition, cured product, circuit board, and semiconductor chip package
[0001] The present invention relates to a resin sheet such as a heat dissipation insulating resin sheet or a heat dissipation resin sheet, a heat dissipation member, a laminate, a resin composition, a cured product, a circuit board, and a semiconductor chip package.
[0002] Thermally conductive resin compositions and resin sheets are widely used as heat dissipation materials, and various types have been proposed. For example, Patent Document 1 discloses an epoxy resin composition containing a liquid epoxy resin (A), a curing agent (B), and an inorganic filler (C), in which the inorganic filler (C) has a particle size (D50) corresponding to 50% of the cumulative particle size distribution on a volume basis of 0.1 μm or more and 0.5 μm or less, and contains α-alumina with an α-crystallization rate of 80% or more.
[0003] Patent Document 2 discloses a semiconductor adhesive used to seal connections in a semiconductor device having a connection structure in which the connection portions of a semiconductor chip and a wiring circuit board are electrically connected to each other, and / or a connection structure in which the connection portions of multiple semiconductor chips are electrically connected to each other. Patent Document 2 discloses that the semiconductor adhesive contains a curable resin component and an alumina filler having an average particle size of 15 μm or less, the alumina filler content being 35 to 75 mass% based on the total amount of the semiconductor adhesive, and the semiconductor adhesive has a thermal conductivity of 0.5 to 1.5 W / mK after curing.
[0004] Patent Document 3 discloses an insulating curable resin composition for printed wiring boards, which contains spherical aluminum oxide particles having a thermal conductivity of 15 W / m·K or more and a curable resin composition, in which the volume occupancy of the aluminum oxide particles is 60% by volume or more relative to the total volume of a cured product of the resin composition for printed wiring boards, and the thermal conductivity of the cured product is 2 W / m·K or more.
[0005] Patent Document 4 discloses a resin composition comprising a liquid epoxy resin, a curing agent, and an alumina filler that has been surface-treated with a silane coupling agent having a specific structure. The resin composition also discloses a resin composition in which the content of the alumina filler that has been surface-treated with the silane coupling agent having the specific structure is 45 to 77 parts by mass per 100 parts by mass of the total mass of all components of the resin composition.
[0006] Patent Document 5 discloses a resin composition for underfill encapsulation application that is applied to a circuit board, mounted with a semiconductor chip, and then cured by heat conduction from above the semiconductor chip. Patent Document 5 also discloses a liquid epoxy resin composition for underfill encapsulation application, characterized in that the resin composition contains, in addition to an epoxy resin and a curing agent, spherical aluminum oxide as an inorganic filler having a maximum particle size of 0.5 μm to 15 μm in a volume content of 5 vol% to 50 vol% relative to the total composition. Patent Document 5 also discloses a liquid epoxy resin composition in which the volume content of the spherical aluminum oxide is 15 vol% to 45 vol%.
[0007] Patent Document 6 discloses an insulating curable resin composition for printed wiring boards, which comprises spherical aluminum oxide particles having a thermal conductivity of 15 W / m K or more and a curable resin composition, wherein the volume occupancy of the aluminum oxide particles is 60% by volume or more relative to the total volume of the cured product, and the cured product has a thermal conductivity of 2 W / m K or more. Patent Document 6 also discloses that the curable resin composition is a thermosetting resin composition, and contains an epoxy compound and / or an oxetane compound, a curing agent and / or a curing catalyst, etc.
[0008] In addition, devices equipped with semiconductor elements, such as power devices, often use insulating heat dissipation substrates to dissipate heat generated during use. The insulating heat dissipation substrates used in power devices require high thermal conductivity as a heat dissipation substrate and high insulation to prevent electrical conduction to the metals above and below the substrate. Therefore, the use of insulating resin sheets containing insulating heat dissipation fillers as insulating heat dissipation substrates has been considered. However, there is a trade-off between thermal conductivity and insulation. For example, a high filling rate of insulating heat dissipation filler improves thermal conductivity but tends to result in poor insulation. Therefore, in order to effectively improve thermal conductivity with a small amount of insulating heat dissipation filler, efforts have also been made to improve the thermal conductivity of the insulating heat dissipation filler itself.
[0009] For example, Patent Document 7 discloses a resin composition containing 90 mass % alumina having an average particle size of 3 μm as a specific example of a resin composition that can provide an insulating layer that is excellent in thermal conductivity and peel strength against a metal layer.
[0010] Furthermore, as electronic devices become smaller and their performance improves, the amount of heat generated increases, leading to a growing demand for high heat dissipation in heat-dissipating resin sheets used in electronic devices. While the thermal conductivity of a heat-dissipating resin sheet can be improved by increasing the inorganic filler filling rate, increasing the inorganic filler filling rate can result in a decrease in flexibility, for example, in a B-stage state before curing. When the flexibility of a heat-dissipating resin sheet decreases, it is prone to problems such as cracking when rolled up during storage or during the process of mounting on a substrate, etc.
[0011] Furthermore, it has been considered to increase the thermal conductivity of heat-dissipating resin sheets by using a matrix resin, and the use of an epoxy resin having a mesogenic skeleton has been considered. Although epoxy resins having a mesogenic skeleton tend to increase thermal conductivity, they tend to crystallize easily, which reduces fluidity and makes them difficult to handle. Therefore, for example, Patent Document 8 discloses an epoxy resin composition that contains, in addition to an epoxy resin having a mesogenic skeleton, a phenolic curing agent having a specific structure, a curing accelerator, and a latent catalyst, in order to achieve high thermal conductivity while improving handleability and moldability.
[0012] Furthermore, for example, Patent Document 9 discloses a high-heat-dissipation insulating resin sheet containing an epoxy resin, a curing agent, and an inorganic filler, in which the epoxy resin is oligomerized to contain a certain amount of dimer and trimer, thereby achieving excellent thermal conductivity and flexibility. Patent Document 2 discloses that an epoxy resin having a mesogenic skeleton can be used as the epoxy resin.
[0013] Japanese Patent Publication No. 2022-060084 International Publication No. 2021 / 200553 International Publication No. 2007 / 020793 Japanese Patent No. 6405209 Japanese Patent No. 4966221 Japanese Patent No. 4920929 Japanese Patent Publication No. 2021-28389 International Publication No. 2021 / 161360 Japanese Patent Publication No. 2012-67205
[0014] In recent years, with the miniaturization and high performance of electrical devices, component-embedded boards, which incorporate various components, have attracted attention. To address the heat generated by the embedded components in component-embedded boards, sheet-shaped heat-dissipating materials containing a large amount of thermal filler in the resin are required. Typically, thermally conductive sheets are laminated to a substrate or other material and then molded using a heat press. However, when a thermally molten sheet is laminated to a substrate, separation between the filler and the resin can occur, particularly in areas such as recesses in the substrate where the molten resin flows first and filler is difficult to fill, resulting in uneven distribution of the filler in certain areas. In such cases, the linear expansion coefficients of the unevenly distributed filler differ from those of other areas, resulting in reduced reliability of the thermally conductive sheet. Furthermore, in recent years, the increasing precision of substrates has led to an increase in the number of fine grooves. To address this, the use of small-particle-sized thermally conductive fillers has been considered. However, the use of small-particle-sized thermally conductive fillers makes such separation more likely to occur.
[0015] Therefore, a first object of the present invention is to provide a resin sheet in which separation of the resin and the thermally conductive filler is suppressed.
[0016] In recent years, thermal insulating resin sheets have been considered for use as component-embedded substrates. When used as component-embedded substrates, the thermal insulating resin sheet must be embedded in the narrow gaps inside the electronic device, making it difficult to use a thermally conductive filler with a large particle size so that the filler can penetrate into the narrow gaps. However, with conventional thermal insulating resin sheets, there are limitations to further improving thermal conductivity when using only a thermally conductive filler with a relatively small particle size without using a thermally conductive filler with a relatively large particle size.
[0017] Therefore, a second object of the present invention is to provide a heat dissipation and insulation resin sheet that has excellent thermal conductivity without using a thermally conductive filler with a relatively large particle size.
[0018] Furthermore, as mentioned above, Patent Document 8 discloses that the fluidity of the resin is improved, resulting in improved handling and moldability. However, this merely improves the fluidity of the resin by oligomerizing the epoxy resin by reacting it with a curing agent during curing, and does not disclose any improvement in the flexibility of the heat-dissipating resin sheet before curing or in the B-stage state. Furthermore, if the dimer and trimer are oligomerized to a fixed amount, as in Patent Document 9, the manufacturing process becomes complicated and impractical. In addition, Patent Document 9 uses an amine curing agent or a phenol novolac curing agent as the curing agent, and therefore there is thought to be room for improvement in thermal conductivity.
[0019] Therefore, a third object of the present invention is to provide a heat-dissipating resin sheet that can improve the thermal conductivity and also maintain good flexibility of the heat-dissipating resin sheet before curing without complicating the manufacturing process.
[0020] As a result of extensive investigation, the present inventors have found that the first problem can be solved by incorporating a certain proportion of a single-crystalline filler as a thermally conductive filler, even when a small particle size filler is highly loaded. That is, the present invention provides the following [1] to
[11] as a first invention.
[0021] [1] A resin sheet containing a resin and a thermally conductive filler, the resin sheet satisfying the following conditions (1) to (3): (1) The content of the thermally conductive filler is 50% by volume or more and 80% by volume or less, based on the total amount of the resin sheet. (2) The average particle diameter of the thermally conductive filler is 2 μm or more and 8 μm or less. (3) The thermally conductive filler contains a monocrystalline filler at 12% by volume or more, based on the total amount of the thermally conductive filler. [2] The resin sheet according to [1], wherein the resin is a thermosetting resin. [3] The resin sheet according to [2], wherein the thermosetting resin contains an epoxy resin. [4] The resin sheet according to any one of [1] to [3], wherein the monocrystalline filler contains α-alumina. [5] The resin sheet according to any one of [1] to [4], wherein the thermally conductive filler is surface-treated with a silane coupling agent, or the resin sheet contains a dispersant. [6] A heat dissipation member formed from the resin sheet according to any one of [1] to [5]. [7] A laminate comprising a support and the resin sheet according to any one of [1] to [5] provided on the support. [8] A circuit board comprising an insulating layer formed from a cured product of the resin sheet according to any one of [1] to [5]. [9] A semiconductor chip package comprising the circuit board according to [8] and a semiconductor chip mounted on the circuit board.
[10] A semiconductor chip package comprising a semiconductor chip encapsulated with the resin sheet according to any one of [1] to [5].
[11] A resin composition comprising a resin and a thermally conductive filler, the resin composition satisfying the following conditions (1) to (3): (1) The content of the thermally conductive filler is 50% by volume or more and 80% by volume or less based on the total amount of the resin composition. (2) The average particle size of the thermally conductive filler is 2 μm or more and 8 μm or less. (3) The thermally conductive filler contains a single-crystal filler in an amount of 12% by volume or more based on the total amount of the thermally conductive filler.
[0022] Furthermore, as a result of extensive investigation, the present inventors have found that the second object can be achieved by using an epoxy resin having a highly oriented mesogen skeleton instead of a filler having a relatively large particle size, thereby improving the heat dissipation of the resin. That is, the present invention provides the following
[12] to
[23] as a second invention.
[0023]
[12] A thermal insulation resin sheet comprising an epoxy resin having a mesogen skeleton, a curing agent, and a thermally conductive filler, wherein the curing agent is at least one selected from the group consisting of a curing agent having a triazine skeleton, a cyanate ester curing agent, and a diamine curing agent, the thermally conductive filler has a thermal conductivity of 20 W / m K or more, a D100 of 10 μm or less, and the thermally conductive filler does not contain a thermally conductive filler having a D100 of more than 10 μm, and the content of the thermally conductive filler is 55% by volume or more and 81% by volume or less, where the total volume of non-volatile components in the resin composition constituting the thermal insulation resin sheet is taken as 100% by volume.
[13] The thermal insulation resin sheet according to
[12] , wherein the curing agent has a melting point of 40° C. or less.
[14] The thermal insulation resin sheet according to
[13] , wherein the curing agent having a melting point of 40°C or less is at least one selected from the group consisting of curing agents having a triazine skeleton and cyanate ester curing agents.
[15] The thermal insulation resin sheet according to
[13] or
[14] , wherein the curing agent having a melting point of 40°C or less is a cyanate ester curing agent.
[16] The thermal insulation resin sheet according to any of
[12] to
[15] , wherein the cyanate ester curing agent has a skeleton containing an aromatic ring.
[17] The thermal insulation resin sheet according to any of
[12] to
[16] , wherein the cyanate ester curing agent has a molecular weight of 500 or less.
[18] The thermal insulation resin sheet according to any of
[12] to
[17] , wherein the epoxy resin has a biphenyl skeleton.
[19] The thermal insulation resin sheet according to any of
[12] to
[18] , wherein the diamine curing agent has a molecular weight of 500 or less and is selected from the group consisting of aromatic compounds and alicyclic compounds.
[20] A laminate comprising a support and the thermal insulation resin sheet according to any one of
[12] to
[19] provided on the support.
[21] A circuit board comprising an insulating layer formed from a cured product of the thermal insulation resin sheet according to any one of
[12] to
[20] .
[22] A semiconductor chip package comprising the circuit board according to
[21] and a semiconductor chip mounted on the circuit board.
[23] A semiconductor chip package including a semiconductor chip sealed with the heat dissipation and insulation resin sheet according to any one of
[12] to
[19] .
[0024] Furthermore, after extensive research, the present inventors have found that the third problem can be solved by incorporating a cyanate ester having a melting point of 40°C or less into a heat-dissipating resin sheet in addition to an epoxy resin having a mesogenic skeleton, and have thus completed the present invention. That is, the present invention provides the following
[24] to
[29] as a third invention.
[24] A heat-dissipating resin sheet comprising an epoxy resin having a mesogenic skeleton and a cyanate ester compound having a melting point of 40°C or less.
[25] The heat-dissipating resin sheet according to
[24] above, in which the cyanate ester compound has a skeleton containing an aromatic ring.
[26] The heat-dissipating resin sheet according to
[24] or
[25] above, in which the molecular weight of the cyanate ester compound is 500 or less.
[27] The heat-dissipating resin sheet according to any one of
[24] to
[26] above, in which the epoxy resin has a biphenyl skeleton.
[28] The heat-dissipating resin sheet according to any one of
[24] to
[27] above, in which an inorganic filler is contained.
[29] A cured product of the heat-dissipating resin sheet according to any one of
[24] to
[28] above.
[0025] According to the first aspect of the present invention, a resin sheet can be provided in which separation of the resin and the thermally conductive filler is suppressed. According to the second aspect of the present invention, a heat-dissipating insulating resin sheet can be provided that has excellent thermal conductivity without using a filler with a relatively large particle size. Furthermore, according to the third aspect of the present invention, a heat-dissipating resin sheet can be provided that improves thermal conductivity and also improves the flexibility of the heat-dissipating resin sheet before curing without complicating the manufacturing process.
[0026] 1 is a schematic cross-sectional view showing an example of a semiconductor chip package; 2 is a schematic view showing a process of laminating a resin sheet on a copper plate in an evaluation of embeddability; 3 is a schematic cross-sectional view showing a through-hole divided into five regions after components of the resin sheet have flowed in; and 4 is a schematic view showing a method of evaluating sheet properties.
[0027] (First Invention) [Resin Sheet] The first invention will be described below with reference to embodiments. The resin sheet of the first invention contains a resin and a thermally conductive filler.
[0028] (Thermal Conductive Filler) The resin sheet of the first invention contains a thermally conductive filler, and the thermally conductive filler contains a single-crystalline filler in an amount of 12% by volume or more based on the total amount of thermally conductive filler. Because single-crystalline fillers have a smooth surface, maintaining a certain level of single-crystalline filler content in the entire thermally conductive filler can help prevent friction between fillers and the resulting decrease in fluidity of the thermally conductive filler, thereby preventing separation between the resin and the thermally conductive filler. On the other hand, if the content of the single-crystalline filler is less than 12% by volume based on the total amount of the resin sheet, it becomes difficult to prevent the separation. From these perspectives, the content of the single-crystalline filler is preferably 15% by volume or more, more preferably 30% by volume or more, and even more preferably 50% by volume or more.
[0029] From the viewpoint of suppressing separation between the resin and the thermally conductive filler, the higher the content of the single-crystalline filler, the better, as long as it is 100% by volume or less based on the total amount of the thermally conductive filler. However, as described below, a thermally conductive filler other than the single-crystalline filler may be contained within a range that suppresses separation between the resin and the thermally conductive filler. In such a case, the content of the single-crystalline filler is, for example, 95% by volume or less, preferably 90% by volume or less, more preferably 85% by volume or less, and even more preferably 80% by volume or less based on the total amount of the thermally conductive filler. Whether or not a thermally conductive filler is a single-crystalline filler can be identified, for example, by X-ray analysis.
[0030] The content of the thermally conductive filler in the resin sheet of the first invention is 50% by volume or more and 80% by volume or less, based on the total volume of the resin sheet. If the content of the thermally conductive filler is less than 50% by volume, the viscosity of the entire resin sheet decreases. For example, when the resin sheet is used for a component-embedded substrate, the resin may penetrate into narrow gaps such as grooves between components, resulting in separation between the resin and the filler. This may also result in a decrease in thermal conductivity. On the other hand, if the content of the thermally conductive filler exceeds 80% by volume, friction between the thermally conductive fillers may occur more easily, resulting in separation between the resin and the filler. Furthermore, the sheet properties of the resin sheet may be reduced, resulting in reduced handleability. In light of the above points, the content of the thermally conductive filler is preferably 52% by volume or more and 77% by volume or less, and more preferably 55% by volume or more and 73% by volume or less.
[0031] The thermally conductive filler contained in the resin sheet of the first invention has an average particle size of 2 μm or more and 8 μm or less. If the average particle size of the thermally conductive filler is less than 2 μm, the surface area of the thermally conductive filler becomes too large, causing friction of the thermally conductive filler, making it difficult for the thermally conductive filler to flow, and there is a risk of separation between the resin and the thermally conductive filler. Furthermore, if the average particle size of the thermally conductive filler exceeds 8 μm, it becomes difficult for the thermally conductive filler to enter narrow gaps, which may result in separation between the resin and the thermally conductive filler. From the above perspectives, the average particle size of the thermally conductive filler is preferably 2.5 μm or more and 7.9 μm or less, and more preferably 2.8 μm or more and 7.8 μm or less.
[0032] The average particle size referred to above refers to the average particle size of all thermally conductive fillers contained in the resin sheet. The average particle size of the thermally conductive filler can be measured by observation using an electron microscope or the like. More specifically, the particle sizes of 100 particles of any thermally conductive filler can be measured using, for example, an electron microscope or an optical microscope, and the average particle size (arithmetic mean value) can be used as the average particle size. Furthermore, when the thermally conductive filler is an agglomerated particle, the average particle size of the agglomerated particle may be within the above range.
[0033] Examples of single crystalline fillers include alumina, diamond, etc. Single crystalline fillers may be used alone or in combination of two or more. Among these, at least one selected from alumina and diamond is preferred, alumina is preferred, and α-alumina is more preferred. When using α-alumina as a single crystalline filler, α-alumina may be used alone as a single crystalline filler, or other single crystalline fillers such as diamond may be used in combination with α-alumina. As-grown diamonds and the like can be used as diamonds that can be used as single crystalline fillers. Note that as-grown diamonds are single crystalline particles that maintain the shape at the time of synthesis without crushing crystalline diamonds obtained by high-temperature and high-pressure methods or the like.
[0034] The thermally conductive filler may include a thermally conductive filler other than a single-crystalline filler. Examples of thermally conductive fillers other than a single-crystalline filler include crushed fillers, polycrystalline fillers, and amorphous fillers. Crushed fillers are fillers obtained by crushing a single-crystalline filler, a polycrystalline filler, an amorphous filler, and the like. Specific examples of thermally conductive fillers include carbides, nitrides, oxides, hydroxides, and carbon-based materials. Examples of carbides include silicon carbide, boron carbide, aluminum carbide, titanium carbide, and tungsten carbide. Examples of nitrides include silicon nitride, boron nitride, aluminum nitride, gallium nitride, chromium nitride, tungsten nitride, magnesium nitride, molybdenum nitride, and lithium nitride. Examples of oxides include zinc oxide, iron oxide, boehmite, aluminum oxide other than alumina (e.g., zinc oxide, iron oxide, boehmite), metal oxides such as magnesium oxide, titanium oxide, cerium oxide, zirconium oxide, and silicon oxide (silica). Examples of hydroxides include metal hydroxides such as aluminum hydroxide, calcium hydroxide, and magnesium hydroxide. Examples of carbon-based materials include diamond other than single-crystalline fillers, carbon black, graphite, graphene, fullerene, carbon nanotubes, and carbon nanofibers. Examples of diamond other than single-crystalline fillers include crushed diamonds obtained by crushing as-grown diamonds. Examples of thermally conductive fillers other than single-crystalline fillers include aluminum oxide, aluminum nitride, diamond, and silicon carbide. Thermally conductive fillers other than single-crystalline fillers may be used alone or in combination of two or more.
[0035] From the viewpoint of effectively improving the heat dissipation properties of the resin sheet, it is preferable to use two or more types of thermally conductive fillers with different average particle sizes in combination, and more preferably to use two types with different average particle sizes in combination. The thermally conductive filler preferably includes, for example, a small-sized thermally conductive filler with an average particle size of 0.05 μm or more and less than 1.5 μm and a large-sized thermally conductive filler with an average particle size of 1.5 μm or more and less than 10 μm. The average particle size of the small-sized thermally conductive filler is preferably 0.1 μm or more and 1 μm or less, and the average particle size of the large-sized thermally conductive filler is preferably 2 μm or more and 8 μm or less. When a small-sized thermally conductive filler and a large-sized thermally conductive filler are used in combination, the mass ratio of the large-sized thermally conductive filler to the mass of the small-sized thermally conductive filler (amount of large-sized thermally conductive filler / amount of small-sized thermally conductive filler) is, for example, 0.5 to 15, preferably 1 to 10, and more preferably 1.5 to 8. It is possible to determine that the resin sheet contains two or more types of thermally conductive fillers with different average particle sizes when two or more peaks appear in the particle size distribution of the thermally conductive fillers.
[0036] (Resin) The resin contained in the resin sheet of the first invention is preferably a curable resin, more preferably a thermosetting resin. Examples of thermosetting resins include amino resins such as urea resins and melamine resins, phenolic resins, thermosetting urethane resins, epoxy resins, silicone resins, phenoxy resins, thermosetting polyimide resins, aminoalkyd resins, benzoxazine resins, and bismaleimide resins. Among these, epoxy resins are preferred.
[0037] Examples of epoxy resins include compounds containing two or more epoxy groups in the molecule. Examples of epoxy resins include those having a weight-average molecular weight of less than 10,000, preferably 5,000 or less. The weight-average molecular weight is the weight-average molecular weight measured in terms of polystyrene by gel permeation chromatography (GPC). Tetrahydrofuran is preferably used as the eluent in gel permeation chromatography (GPC) measurements. However, when the molecular weight is low, 1,000 or less, the weight-average molecular weight can be calculated from the structural formula. In addition, although the epoxy resin in the resin sheet may have reacted by curing, the weight-average molecular weight refers to the weight-average molecular weight of the epoxy resin in a state before curing.
[0038] Specific examples of epoxy resins include mesogenic epoxy resins such as styrene-based epoxy resins, resorcinol-based epoxy resins, bisphenol A-based epoxy resins, bisphenol F-based epoxy resins, bisphenol S-based epoxy resins, phenol novolac-based epoxy resins, biphenol-based epoxy resins, phenoxy-based epoxy resins, naphthalene-based epoxy resins, phenylene ether-based epoxy resins, fluorene-based epoxy resins, phenol aralkyl-based epoxy resins, naphthol aralkyl-based epoxy resins, dicyclopentadiene-based epoxy resins, anthracene-based epoxy resins, and biphenyl-based epoxy resins, as well as epoxy resins having an adamantane skeleton, epoxy resins having a tricyclodecane skeleton, and epoxy resins having a triazine nucleus in the skeleton, and glycidylamine-based epoxy resins. Among these, at least one selected from bisphenol A-based epoxy resins, bisphenol F-based epoxy resins, dicyclopentadiene-based epoxy resins, and epoxy resins having a mesogenic skeleton is preferred. Among these, at least one selected from bisphenol A type epoxy resins, bisphenol F type epoxy resins, and dicyclopentadiene type epoxy resins is more preferred.
[0039] The epoxy equivalent of the epoxy resin is not particularly limited, but is, for example, 100 g / eq or more and 1000 g / eq or less. The epoxy equivalent of the epoxy resin is preferably 120 g / eq or more, more preferably 140 g / eq or more, and is preferably 500 g / eq or less, more preferably 400 g / eq or less. The epoxy equivalent can be measured, for example, according to the method specified in JIS K 7236.
[0040] As the resin, a polymer having a weight-average molecular weight of, for example, 10,000 or more may be used. The use of a polymer facilitates improving the sheetability of the resin sheet. The polymer may be a thermosetting resin or a resin other than a thermosetting resin, but a thermosetting resin is preferred. The polymer may also have a functional group such as an epoxy group or a hydroxyl group. The polymer is preferably used in combination with a thermosetting resin (hereinafter sometimes referred to as "resin (A)") having a weight-average molecular weight of, for example, less than 10,000, and is particularly preferably used in combination with an epoxy resin as resin (A). The weight-average molecular weight of resin (A) is preferably 5,000 or less.
[0041] Specific examples of polymers include phenoxy resins, polyester resins, polyether resins, polyamide resins, polyamideimide resins, polyimide resins, polyvinyl butyral resins, polyvinyl formaldehyde resins, polyhydroxypolyether resins, polystyrene resins, polycarbonate resins, butadiene resins, acrylonitrile-butadiene copolymers, acrylonitrile-butadiene-styrene resins, and styrene-butadiene copolymers. Among these, phenoxy resins are preferred. Examples of phenoxy resins include those having a skeleton such as a bisphenol A skeleton, a bisphenol F skeleton, a bisphenol S skeleton, a bisphenolacetophenone skeleton, a novolac skeleton, a biphenyl skeleton, a fluorene skeleton, a dicyclopentadiene skeleton, a norbornene skeleton, a naphthalene skeleton, an anthracene skeleton, an adamantane skeleton, a terpene skeleton, a trimethylcyclohexane skeleton, or an imide skeleton. The phenoxy resin may or may not have an epoxy group.
[0042] Commercially available examples of the phenoxy resin include "YP-50S", "YP55", and "YP70" (all manufactured by Nippon Steel Chemical & Material Co., Ltd.), "JER1256", "JER4250", "JER4275", "YX6954BH30", "YX6954BH30", "YX7553", "YX7553BH30", "YL7769BH30", "YL6794", "YL7213", "YL7290", "YL7891BH30", and "YL7482" (all manufactured by Mitsubishi Chemical Corporation).
[0043] The weight average molecular weight of the polymer is not particularly limited, but is preferably 20,000 or more, more preferably 35,000 or more, and preferably 100,000 or less, more preferably 80,000 or less, and even more preferably 70,000 or less.
[0044] In the resin sheet of the first invention, when a polymer is used, it is preferably used in combination with resin (A). When resin (A) and a polymer are used in combination, the mass ratio of resin (A) / polymer is not particularly limited, but is, for example, 0.1 or more and 10 or less, preferably 0.2 or more and 8 or less, more preferably 0.3 or more and 7 or less, and even more preferably 0.2 or more and 8 or less. The resin (A) and the polymer may be used alone or in combination of two or more.
[0045] The content of the resin (A) is, for example, 20% by mass or more and 80% by mass or less, preferably 30% by mass or more and 75% by mass or less, more preferably 35% by mass or more and 70% by mass or less, and even more preferably 40% by mass or more and 65% by mass or less, based on the total amount of components of the resin sheet excluding the thermally conductive filler. The total content of the resin (A) and the polymer is, for example, 20% by mass or more and 90% by mass or less, preferably 30% by mass or more and 85% by mass or less, more preferably 35% by mass or more and 80% by mass or less, and even more preferably 40% by mass or more and 75% by mass or less, based on the total amount of components of the resin sheet excluding the thermally conductive filler.
[0046] (Curing Agent) The resin sheet of the first invention may contain a curing agent as needed. The curing agent is preferably contained together with the thermosetting resin, and more preferably together with the epoxy resin. For example, when the resin sheet contains an epoxy resin, the curing agent preferably contains at least one selected from a curing agent having a triazine skeleton, a cyanate ester curing agent, a diamine curing agent, a phenolic curing agent, an amine curing agent, an acid anhydride curing agent, a mercaptan curing agent, and an imidazole curing agent. Among these, it is more preferable to contain at least one selected from a curing agent having a triazine skeleton, a cyanate ester curing agent, a diamine curing agent, and an acid anhydride curing agent. Using these as curing agents makes it easier to impart excellent thermal conductivity to the resin sheet.
[0047] <Curing Agent Having a Triazine Skeleton> Examples of curing agents having a triazine skeleton include phenolic compounds, amine compounds, thiol compounds, imidazole compounds, and phosphine compounds having a triazine skeleton. Among these, phenolic compounds having a triazine skeleton are preferred. Furthermore, as the curing agent having a triazine skeleton, compounds having an aminotriazine skeleton are more preferred. The triazine skeleton of a curing agent enhances alignment and tends to improve thermal conductivity. Examples of phenolic compounds having a triazine skeleton include novolac-type phenolic compounds, and more specifically, novolac-type phenolic resins modified with melamine, benzoguanamine, or the like. Examples of phenolic compounds having a triazine skeleton include "Phenolite (registered trademark) LA-7052," "Phenolite (registered trademark) LA-7054," "Phenolite (registered trademark) LA-7751," "Phenolite (registered trademark) LA-1356," and "Phenolite (registered trademark) LA-3018-50P" (all manufactured by DIC Corporation). The curing agent having a triazine skeleton may be used alone or in combination of two or more kinds.
[0048] <Cyanate Ester-Based Curing Agent> A cyanate ester-based curing agent is a compound having a cyanate ester group (—OCN). The cyanate ester-based curing agent is a compound that functions as a curing agent for, for example, epoxy resins. A portion of the cyanate ester group trimers during curing to form a triazine skeleton, which, after curing, forms a molecular structure with high alignment together with the resin, making it easier to improve thermal conductivity. Furthermore, from the perspective of improving curability, it is preferable for the cyanate ester-based curing agent to have two or more cyanate ester groups per molecule. From the perspective of increasing the alignment of the molecular structure to easily improve thermal conductivity and to easily lower the melting point, it is preferable for the cyanate ester-based curing agent to have two to three cyanate ester groups per molecule, and more preferably two.
[0049] The cyanate ester curing agent preferably has a skeleton containing an aromatic ring, and more preferably has a skeleton containing a phenyl ring. Having a skeleton containing an aromatic ring improves the alignment after curing, making it easier to further improve the thermal conductivity after curing. Furthermore, the cyanate ester curing agent preferably has the cyanate ester group directly bonded to the aromatic ring, and more preferably directly bonded to the phenyl ring. Direct bonding of the cyanate ester group to the aromatic ring makes it easier to increase the reactivity of the cyanate ester group, making it easier for trimerization and curing to proceed by heating.
[0050] The molecular weight of the cyanate ester curing agent is preferably 500 or less. A molecular weight of 500 or less facilitates the curing reaction with the resin, making it easier to obtain a resin sheet with excellent thermal conductivity. Furthermore, the melting point of the cyanate ester curing agent tends to be below a certain level, improving the sheetability of the resin sheet and making it easier to prevent cracks from occurring when the resin sheet is wound into a roll, for example. The molecular weight of the cyanate ester curing agent is more preferably 400 or less, and even more preferably 320 or less. The molecular weight of the cyanate ester curing agent is not particularly limited, but may be, for example, 150 or more, or 200 or more.
[0051] Examples of cyanate ester curing agents include bisphenol cyanate esters. The bisphenol cyanate esters preferably have a bisphenol skeleton and a structure in which one cyanate ester group is directly bonded to each phenyl group of the bisphenol skeleton. Examples of bisphenol cyanate esters include bisphenol cyanate ester resins such as bisphenol A cyanate ester resins, bisphenol E cyanate ester resins, and bisphenol F cyanate ester resins. Among these, bisphenol E cyanate ester resins are preferred. The cyanate ester curing agent may be a partial or complete trimerization of the bisphenol cyanate ester (trimeric cyanate ester), but from the viewpoint of lowering the molecular weight and melting point, monomeric bisphenol cyanate esters are preferred. The cyanate ester curing agents may be used alone or in combination of two or more. As the cyanate ester-based curing agent, commercially available products can be used, such as "P-201" manufactured by Mitsubishi Gas Chemical Company, Inc., and "BA-230S," "BA-3000S," "BTP-1000S," and "BTP-6020S" manufactured by Lonza Japan Ltd.
[0052] <Diamine-based curing agent> Examples of diamine-based curing agents include compounds having two amino groups. Here, the amino group may be either a primary amino group or a secondary amino group, but a primary amino group is preferred from the viewpoint of reactivity. Therefore, it is preferable for the amine-based curing agent to have two primary amino groups. Furthermore, examples of diamine-based curing agents include aromatic compounds or alicyclic compounds from the viewpoint of improving alignment and thermal conductivity, and aromatic compounds are preferred from the viewpoint of reactivity and improving alignment and thermal conductivity. Examples of aromatic compounds include aromatic compounds having an aromatic ring, preferably a phenyl group, in the molecule. Specific examples include aromatic amines in which an amino group is directly bonded to an aromatic ring, such as m-phenylenediamine, p-phenylenediamine, tolylene-2,4-diamine, tolylene-2,6-diamine, mesitylene-2,4-diamine, mesitylene-2,6-diamine, 3,5-diethyltolylene-2,4-diamine, 3,5-diethyltolylene-2,6-diamine, biphenylenediamine, 4,4-diaminodiphenylmethane, 2,5-naphthylenediamine, and 2,6-naphthylenediamine, and amines in which an amino group is not directly bonded to an aromatic ring, such as m-xylylenediamine, p-xylylenediamine, and a reaction product of m-xylylenediamine and styrene. Among these, aromatic amines in which an amino group is directly bonded to an aromatic ring are more preferred from the viewpoint of reactivity. Examples of the alicyclic compound include alicyclic polyamines such as 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, cyclohexanediamine, methylcyclohexanediamine, isophoronediamine, 4,4'-methylenebis(N-sec-butylcyclohexaneamine), etc. The diamine curing agent may be used alone or in combination of two or more.
[0053] The molecular weight of the diamine curing agent is preferably 500 or less, more preferably 300 or less, and even more preferably 250 or less. When the molecular weight of the diamine curing agent is equal to or less than the upper limit, the amount of curing agent present is reduced, and as a result, the amount of resin present is increased, making it easier to obtain a resin sheet with excellent thermal conductivity. The molecular weight of the diamine curing agent is not particularly limited, but may be, for example, 100 or more, preferably 150 or more, and more preferably 170 or more.
[0054] <Acid anhydride curing agent> Examples of acid anhydride curing agents include phthalic anhydride, hexahydrophthalic anhydride, 4-methylhexahydrophthalic anhydride, tetrahydrophthalic anhydride, 4-methyltetrahydrophthalic anhydride, tetrabromophthalic anhydride, etc. The acid anhydride curing agents may be used alone or in combination of two or more.
[0055] The content of the curing agent is preferably 10 parts by mass or more and 150 parts by mass or less, more preferably 15 parts by mass or more and 120 parts by mass or less, and even more preferably 20 parts by mass or more and 110 parts by mass or less, relative to 100 parts by mass of the resin. When the content of the curing agent is above the lower limit, the curing reaction with the resin proceeds sufficiently, making it easier to obtain a resin sheet with excellent sheetability. Furthermore, when the content of the curing agent is below the upper limit, the curing reaction with the resin can proceed without excessive curing agent being contained, making it easier to suppress bleed-out of the curing agent. Furthermore, as a result of increasing the amount of resin present, it becomes easier to obtain a resin sheet with excellent thermal conductivity.
[0056] When the resin sheet contains an epoxy resin and a curing agent, the ratio of the equivalent of the curing agent to the equivalent of the epoxy resin (equivalent of curing agent / equivalent of epoxy resin) is not particularly limited, but is, for example, 0.3 or more and 2 or less, preferably 0.4 or more and 1.5 or less, and more preferably 0.5 or more and 1.2 or less.
[0057] (Curing accelerator) The resin sheet of the first invention may contain a curing accelerator. By containing a curing accelerator, the curing property of the resin sheet can be improved. The curing accelerator is not particularly limited, and examples thereof include imidazole-based curing accelerators, organic phosphine-based curing accelerators, and tertiary amine-based curing accelerators. Among them, it is preferable to use at least one selected from imidazole-based curing accelerators and organic phosphine-based curing accelerators.
[0058] Examples of the imidazole curing accelerator include 1-cyanoethyl-2-phenylimidazole in which the 1-position of imidazole is protected with a cyanoethyl group, and imidazole curing accelerators in which the basicity is protected with isocyanuric acid. Examples of commercially available products include 2MA-OK, 2MZ, 2MZ-P, 2PZ, 2PZ-PW, 2P4MZ, C11Z-CNS, 2PZ-CN, 2PZ-CNS, 2PZCNS-PW, 2MZ-A, 2MZA-PW, C11Z-A, 2E4MZ-A, 2MAOK-PW, 2PZ-OK, 2MZ-OK, 2PHZ, 2PHZ-PW, 2P4MHZ, 2P4MHZ-PW, 2E4MZ-BIS, VT, VT-OK, MAVT, and MAVT-OK (all manufactured by Shikoku Chemicals Corporation).
[0059] Examples of organic phosphine curing accelerators include triphenylphosphine, tetraphenylphosphonium tetra-p-tolylborate, tetraphenylphosphonium tetraphenylborate, tri-tert-butylphosphonium tetraphenylborate, (4-methylphenyl)triphenylphosphonium thiocyanate, tetraphenylphosphonium thiocyanate, butyltriphenylphosphonium thiocyanate, triphenylphosphine triphenylborane, etc. Examples of commercially available products include TPP, TPP-MK, TPP-K, TTBuP-K, TPP-SCN, and TPP-S (all manufactured by Hokko Chemical Industry Co., Ltd.).
[0060] The above curing accelerators may be used alone or in combination of two or more. The content of the curing accelerator is, for example, 0.3 parts by mass or more and 7 parts by mass or less, preferably 0.5 parts by mass or more and 5 parts by mass or less, and more preferably 0.7 parts by mass or more and 3 parts by mass or less, relative to 100 parts by volume of the total amount of the resin and the curing agent.
[0061] (Dispersant) The resin sheet of the first invention preferably contains a dispersant. The dispersant is blended into the resin together with the thermally conductive filler, etc., to improve the dispersibility of the thermally conductive filler and more easily prevent separation between the resin and the thermally conductive filler. A silane coupling agent is preferably used as the dispersant. When using a silane coupling agent, it is preferable to surface treat the thermally conductive filler with the silane coupling agent, as described below. As the silane coupling agent, for example, an alkoxysilane compound can be used. An alkoxysilane compound is a compound having a structure in which one to three of the four bonds possessed by a silicon atom (Si) are bonded to alkoxy groups, and the remaining bond is bonded to an organic substituent. The alkoxy group possessed by the alkoxysilane compound is a hydrolyzable group, such as a methoxy group, an ethoxy group, a protoxy group, a butoxy group, a pentoxy group, and a hexatoxy group. Among these, an alkoxysilane compound having a methoxy group or an ethoxy group is preferred. From the viewpoint of increasing affinity with the thermally conductive filler, the number of alkoxy groups in the alkoxysilane compound is preferably 3. Therefore, the alkoxysilane compound is more preferably at least one selected from a trimethoxysilane compound and a triethoxysilane compound.
[0062] Examples of functional groups contained in the organic substituent of the alkoxysilane compound include an acryloyl group, an alkyl group, a carboxyl group, a vinyl group, a methacrylic group, an aromatic group, an amino group, an isocyanate group, an isocyanurate group, an epoxy group, a hydroxyl group, and a mercapto group. By appropriately selecting the functional group, compatibility with the resin can be improved. From this perspective, for example, when the resin contains an epoxy resin, the functional group is preferably an epoxy group.
[0063] In addition, the alkoxysilane compound is preferably an alkylalkoxysilane compound having an alkyl group bonded to a silicon atom, from the viewpoint of improving compatibility with the resin and enhancing the dispersibility of the thermally conductive filler. The number of carbon atoms in the alkyl group bonded to the silicon atom is preferably 4 or more. In addition, the number of carbon atoms in the alkyl group bonded to the silicon atom is preferably 16 or less, from the viewpoint of keeping the viscosity of the alkoxysilane compound itself relatively low and keeping the viscosity of the resin composition low. In addition, the alkoxysilane compound may be a polymeric silane compound having a polyorganosiloxane skeleton and an alkoxysilyl group.
[0064] Preferred alkylalkoxysilane compounds include n-hexyltrimethoxysilane, n-hexyltriethoxysilane, n-octyltriethoxysilane, and n-decyltrimethoxysilane. Examples of alkoxysilane compounds other than alkylalkoxysilane compounds include 3-acryloxypropyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-isocyanatopropyltriethoxysilane, 3-(2-aminoethyl)aminopropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, glycidoxypropyltrimethoxysilane, and 3-phenylaminopropyltrimethoxysilane.
[0065] As the dispersant, a dispersant other than a silane coupling agent may be used. Examples of dispersants other than silane coupling agents that can be used include polymeric dispersants other than silicone compounds. Examples of the polymeric dispersant that can be used include polymeric compounds having functional groups. Examples of polymeric compounds include acrylic, vinyl, polyester, polyurethane, polyether, epoxy, polystyrene, and amino compounds. Examples of functional groups include carboxyl groups, phosphoric acid groups, sulfonic acid groups, carboxylic acid ester groups, phosphoric acid ester groups, sulfonic acid ester groups, hydroxyl groups, amino groups, quaternary ammonium bases, and amide groups.
[0066] As the dispersant other than the silane coupling agent, commercially available products may be used, for example, Phosphanol (registered trademark) RA-600, ML-200, ML-220, RS-610, RB-410, RD-720N (all manufactured by Toho Chemical Industry Co., Ltd.), Solsperse (registered trademark) SOLSPERSE 26000, SOLSPERSE 36000, SOLSPERSE 41000 (all manufactured by ZENECA), DISPERBYK " (registered trademark)-110, 111, 142, 145, 180, "BYK" (registered trademark)-110, 111, W969, W9010 (all manufactured by BYK Japan KK), Plysurf (registered trademark) A-208B, A-208F, A-208N, A-219B, DB-01, M208F (all manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.), Disparlon (registered trademark) PW-36, DA-375 (all manufactured by Kusumoto Chemicals Co., Ltd.), and the like can be used.
[0067] The content of the dispersant in the resin sheet is not particularly limited, but is, for example, 0.5% by mass to 15% by mass, preferably 1% by mass to 10% by mass, and more preferably 2% by mass to 5% by mass, based on the total amount of components of the resin sheet excluding the thermally conductive filler. Note that, as the dispersant, one of the above-mentioned dispersants may be used alone, or two or more of them may be used in combination.
[0068] In the above description, when the thermally conductive filler is surface-treated with a silane coupling agent, an embodiment is shown in which the thermally conductive filler is surface-treated with a silane coupling agent blended in a resin. However, the thermally conductive filler may be surface-treated with a silane coupling agent in advance and then mixed with a resin. By surface-treating the thermally conductive filler in advance with a silane coupling agent, the thermally conductive filler is surface-modified in advance with the silane coupling agent, and separation from the resin is more likely to be suppressed. The thermally conductive filler that has been surface-modified in advance may be mixed with a resin to produce a resin composition.
[0069] The method for pre-surface treatment using a silane coupling agent is not particularly limited, and may be any known method, for example, a wet treatment method, a dry treatment method, etc. In the wet treatment method, for example, a thermally conductive filler is added to and mixed with a treatment liquid in which a dispersant is dispersed or dissolved in a solvent, and then the mixture is dried, heated, washed, etc., to bond or adhere the silane coupling agent to the surface of the thermally conductive filler. In addition, the dry treatment method is a surface treatment method that does not use a solvent, and specifically, a dispersant is mixed with the thermally conductive filler, stirred with a mixer, etc., and then heated to bond or adhere the silane coupling agent to the surface of the thermally conductive filler.
[0070] [Other Components] In addition to the above components, the resin sheet of the first invention may contain other additives such as a flame retardant, an antioxidant, a tackifier, a plasticizer, a thixotropy imparting agent, and a colorant. Furthermore, a solvent may be blended into the resin sheet during its manufacturing method, and it is preferable that the blended solvent partially remains in the resin sheet.
[0071] The resin sheet of the first invention may be in an uncured or semi-cured state. When the resin sheet is in an uncured or semi-cured state, it has high adhesion to another member and can be adhered to another member with high adhesive strength.
[0072] [Thickness] The thickness of the resin sheet is not particularly limited, but is, for example, 10 μm or more and 500 μm or less. A thickness of 10 μm or more ensures a certain level of heat dissipation, while a thickness of 500 μm or less makes it easier to thin electronic devices to which the resin sheet is applied, such as circuit boards and semiconductor devices, and is particularly suitable for use in component-embedded substrates. The thickness of the resin sheet is preferably 15 μm or more, more preferably 20 μm or more, and preferably 400 μm or less, more preferably 260 μm or less.
[0073] [Thermal Conductivity] The thermal conductivity of the resin sheet is preferably 0.2 W / (m·K) or more. A thermal conductivity of 0.2 W / (m·K) or more improves heat dissipation. From the viewpoint of heat dissipation, the thermal conductivity is more preferably 0.3 W / (m·K) or more, and even more preferably 0.5 W / (m·K) or more. As described above, increasing the thermal conductivity improves heat dissipation, and when used as a circuit board or a component-embedded board, heat generated by electronic components mounted on the circuit board or embedded within the resin sheet can be efficiently dissipated to the outside. The upper limit of the thermal conductivity of the resin sheet is not particularly limited, but in practice it is, for example, about 30 W / (m·K). The thermal conductivity of the resin sheet can be determined as described in the examples below.
[0074] [Laminate] The resin sheet of the first invention may be used in a laminate, which may include a support and a resin sheet provided on the support.
[0075] Examples of the support include a resin film made of a plastic material, a metal foil, and release paper, with a resin film made of a plastic material being preferred. When a resin film made of a plastic material is used as the support, examples of the plastic material include polyesters such as polyethylene terephthalate (hereinafter sometimes abbreviated as "PET") and polyethylene naphthalate (hereinafter sometimes abbreviated as "PEN"), polycarbonate (hereinafter sometimes abbreviated as "PC"), acrylics such as polymethyl methacrylate (PMMA), cyclic polyolefins, triacetyl cellulose (TAC), polyether sulfide (PES), polyether ketone, polyimide, and the like. Among these, polyethylene terephthalate and polyethylene naphthalate are preferred, with inexpensive polyethylene terephthalate being particularly preferred.
[0076] When a metal foil is used as the support, examples of the metal foil include copper foil and aluminum foil, with copper foil being preferred. The copper foil may be a foil made of a single metal, such as copper, or a foil made of an alloy of copper and another metal (e.g., tin, chromium, silver, magnesium, nickel, zirconium, silicon, titanium, etc.).
[0077] The support may be subjected to a matte treatment or a corona treatment on the surface to be bonded to the resin sheet. Alternatively, the support may be a support with a release layer, which has a release layer on the surface to be bonded to the resin sheet. Examples of the release agent used in the release layer of the support with a release layer include one or more release agents selected from the group consisting of alkyd resins, polyolefin resins, urethane resins, and silicone resins.
[0078] The thickness of the support is not particularly limited, but is, for example, in the range of 1 to 80 μm, preferably in the range of 5 to 75 μm, and more preferably in the range of 10 to 60 μm. When a support with a release layer is used, it is preferable that the thickness of the entire support with a release layer is in the above range.
[0079] In the laminate, a protective film can be further laminated on the surface of the resin composition layer (resin sheet) that is not bonded to the support (i.e., the surface opposite to the support). The protective film can be the same as the support, and a resin film can be preferably used. By laminating the protective film, it is possible to prevent adhesion of dust and scratches to the surface of the resin composition layer. The resin sheet or laminate can be wound up into a roll and stored. When the resin sheet (i.e., the laminate) has a protective film, it can be used by peeling off the protective film.
[0080] [Resin Composition] The resin composition according to the first invention contains a resin and a thermally conductive filler, and like the resin sheet, satisfies the following conditions (1) to (3): (1) The content of the thermally conductive filler is 50% by volume or more and 80% by volume or less based on the total amount of the resin composition. (2) The average particle size of the thermally conductive filler is 2 μm or more and 8 μm or less. (3) The thermally conductive filler contains a single-crystalline filler in an amount of 12% by volume or more based on the total amount of the thermally conductive filler.
[0081] The resin composition of the first invention may contain, in addition to the resin and thermally conductive filler, other additives such as the above-mentioned curing agent, curing accelerator, dispersant, flame retardant, antioxidant, tackifier, plasticizer, thixotropy imparting agent, and colorant. Details of each component in the resin composition are as described for the resin sheet, so detailed description of these is omitted. However, when the content of each component is described based on the total amount of the resin sheet, in the resin composition, it is based on the total amount of the resin composition.
[0082] (Method for manufacturing resin sheet and laminate) The resin sheet can be obtained by molding a resin composition into a sheet. The resin composition can be obtained by mixing, in addition to the resin and thermally conductive filler, various additives such as a dispersant, a curing agent, a curing accelerator, and the like, which are optionally blended. The resin composition may also be diluted with a dilution solvent such as an organic solvent. The thermally conductive filler may also be surface-treated in advance with a surface treatment agent such as a silane coupling agent as described above, and then mixed with the resin.
[0083] The method for forming the resin composition into a sheet is not particularly limited. For example, the resin composition may be coated or laminated on a release sheet, metal foil, or support, and then dried by heating or other means as needed to form a sheet. The term "sheet-like" or "sheet" refers to a thin, flat object whose thickness is small relative to its length and width. The concept of a sheet also includes a film or layer formed on another member, such as a support. As explained above, a laminate can be obtained by forming a resin sheet on a support. The resin composition formed into a sheet (resin sheet) may be heated and semi-cured to a B-stage state as needed.
[0084] Examples of organic solvents used as the diluent include ketones such as acetone, methyl ethyl ketone (MEK), and cyclohexanone, acetate esters such as ethyl acetate, butyl acetate, cellosolve acetate, propylene glycol monomethyl ether acetate, and carbitol acetate, carbitols such as cellosolve and butyl carbitol, aromatic hydrocarbons such as toluene and xylene, and amide solvents such as dimethylformamide, dimethylacetamide (DMAc), and N-methylpyrrolidone. These organic solvents may be used alone or in combination of two or more.
[0085] (Method of using the resin sheet) The resin sheet may be cured and used as a cured product for various purposes. The resin sheet may be laminated in the uncured or semi-cured state onto an adherend such as a metal base plate, other substrate, or electronic component, and cured to be adhered to the adherend. The resin sheet may be used for various purposes requiring heat dissipation. That is, the first invention also provides a heat dissipation member formed from the resin sheet. In particular, it is preferably used as a heat dissipation member for electronic devices, and more preferably used in semiconductor devices.
[0086] More specifically, the resin sheet may be used as part of a circuit board or as an encapsulant for electronic components for embedding electronic components such as semiconductor chips. Among these, the resin sheet is preferably used as an encapsulant. The circuit board is preferably a component-embedded substrate. Component-embedded substrates generally have narrow gaps. When resin sheets are laminated in an uncured or semi-cured state, the resin tends to penetrate into the narrow gaps first, causing separation between the resin and the thermally conductive filler. However, the resin sheet of the present invention contains a predetermined amount of a thermally conductive filler with a relatively small average particle size and a certain proportion or more of a monocrystalline filler, thereby suppressing the separation and making the resin sheet suitable for use in component-embedded substrates with narrow gaps. The circuit board is preferably used in a semiconductor package. The semiconductor chip package includes a circuit board and a semiconductor chip mounted on the circuit board. In the semiconductor chip package, the semiconductor chip is preferably encapsulated with the resin sheet of the first invention described above.
[0087] FIG. 1 shows an example of a semiconductor package using the resin sheet of the first invention. As shown in FIG. 1, for example, a semiconductor chip package 100 includes a semiconductor chip 110, a sealing layer 120 formed to cover the periphery of the semiconductor chip 110, and a resin layer 130 provided on the surface of the semiconductor chip 110 opposite the side covered by the sealing layer. The sealing layer 120 may be formed from the resin sheet of the first invention. The sealing layer 120 may be an insulating layer. The resin layer 130 may be, for example, an insulating layer formed from a known resin material or a thermally conductive resin composition. In the semiconductor package 100, the resin layer 130 may be provided with a conductive layer 140 electrically connected to the semiconductor chip 110, a solder resist layer 150, bumps 160 further connected to the conductive layer 140, and the like. However, the configuration of the semiconductor chip package shown in FIG. 1 is merely an example, and specific examples of semiconductor chip packages are not limited to the configuration shown in FIG. 1.
[0088] As described above, an example of a method for encapsulating an electronic component such as a semiconductor chip in a resin sheet using a resin sheet as an encapsulant is as follows. The semiconductor chip package described above may be manufactured by the following method, but the manufacturing method for the semiconductor chip package is not limited to the following method. First, a fixing film to which an electronic component such as a semiconductor chip, or an electronic component and a substrate, is fixed is prepared. The fixing film may have an adhesive layer on one side, and the electronic component and the substrate may be fixed via the adhesive layer. Next, a resin sheet may be laminated on one side of the fixing film, embedding the electronic component, or the electronic component and the substrate, etc., inside the resin sheet, and laminating the resin sheet on the fixing film. The resin sheet with the electronic component, or the electronic component and the substrate, etc. embedded inside it as described above is cured by heating to become a cured product, and an electronic component such as a semiconductor chip may be embedded inside it and used as a component-embedded substrate. Furthermore, the resin sheet with the electronic component embedded inside as described above may be peeled off from the fixing film as appropriate, and another component (e.g., the resin layer described above) may be formed on the surface from which the fixing film was peeled off. The resin sheet may be cured after the fixing film is peeled off, or may be cured on the fixing film.
[0089] (Second Invention) [Heat Dissipation / Insulation Resin Sheet] Hereinafter, the second invention will be described with reference to embodiments. The heat dissipation / insulation resin sheet of the second invention contains an epoxy resin having a mesogenic skeleton, a curing agent, and a thermally conductive filler.
[0090] <Thermal Conductive Filler> The thermal insulating resin sheet according to the second aspect of the present invention contains a thermally conductive filler. The thermally conductive filler has a particle diameter (D100) of 10 μm or less when the cumulative volume is 100%, and does not contain thermally conductive fillers with a D100 of more than 10 μm. If the D100 of the thermally conductive filler exceeds 10 μm, the thermally conductive resin sheet cannot be embedded in narrow gaps inside electronic devices, making it unusable for, for example, component-embedded substrates.
[0091] Furthermore, the thermally conductive filler contained in the thermal insulation resin sheet according to the second aspect of the present invention has a thermal conductivity of 20 W / (m·K) or more. A thermal conductivity of less than 20 W / (m·K) would not sufficiently improve the thermal conductivity of the thermal insulation resin sheet. From this perspective, the thermal conductivity of the thermally conductive filler is preferably 30 W / (m·K) or more. The upper limit of the thermal conductivity of the thermally conductive filler is not particularly limited, but may be, for example, 2000 W / (m·K) or less or 1000 W / (m·K) or less. The thermal conductivity of the thermally conductive filler can be measured, for example, by a cyclic heating thermoreflectance method using a thermal microscope manufactured by Bethel Co., Ltd., on a filler cross section machined with a cross-section polisher.
[0092] Furthermore, the content of the thermally conductive filler in the thermal insulation resin sheet is 55% by volume or more and 81% by volume or less, assuming that the non-volatile components in the resin composition constituting the thermal insulation resin sheet are 100% by volume. If the content of the thermally conductive filler is less than 55% by volume, sufficient thermal conductivity cannot be achieved. If the content of the thermally conductive filler is more than 81% by volume, the epoxy resin having a mesogenic skeleton cannot be sufficiently contained, and thermal conductivity cannot be sufficiently improved. Furthermore, it becomes difficult to disperse the thermally conductive filler in the resin composition. From these viewpoints, the content of the thermally conductive filler is preferably 56% by volume or more and 80% by volume or less, and more preferably 65% by volume or more and 79% by volume or less.
[0093] The thermally conductive filler may have electrical insulation properties, and may have an electrical resistivity of, for example, 10 8 It is preferable that the filler has a resistance to heat of 1000 kJ / cm or more. High electrical insulation properties make it suitable for use in electronic devices such as substrates. Therefore, it is preferable that the thermally conductive filler is a thermally conductive filler having electrical insulation properties.
[0094] Examples of thermally conductive fillers include metal oxides, metal nitrides, metal hydroxides, carbon materials, oxides, nitrides, and carbides other than metals. The thermally conductive filler may be shaped in any form, such as flakes, spheres, crushed particles, irregular shapes, polyhedral shapes, or fibers, or may be in the form of aggregated particles formed by aggregation of primary particles. For example, boron nitride, which will be described later, is preferably used as aggregated particles. Examples of metal oxides in thermally conductive fillers include aluminum oxide (represented by alumina), magnesium oxide, and zinc oxide, and examples of metal nitrides include aluminum nitride. Examples of metal hydroxides include aluminum hydroxide. Examples of carbon materials include spherical graphite, flake graphite, and carbon fiber. Examples of oxides, nitrides, and carbides other than metals include quartz, boron nitride, and silicon carbide. Among these, metal oxides, metal hydroxides, and nitrides are preferred. Specific examples of these thermally conductive fillers include aluminum oxide, aluminum hydroxide, and boron nitride, with alumina being even more preferred. The thermally conductive filler may be used alone or in combination of two or more of the above.
[0095] The thermally conductive filler may have an average particle size of less than 10 μm, preferably 8 μm or less, more preferably 5 μm or less, and even more preferably 4 μm or less. When the average particle size of the thermally conductive filler is equal to or less than the above upper limit, the thermally conductive filler can be highly packed into the thermal insulation resin sheet, making it easier to sufficiently improve thermal conductivity. Furthermore, from the viewpoint of making it easier to exhibit thermal conductivity by having a certain size, the thermally conductive filler preferably has an average particle size of 0.05 μm or more, more preferably 0.1 μm or more, and even more preferably 0.2 μm or more.
[0096] The average particle size of the thermally conductive filler can be measured by observation using an electron microscope or the like. More specifically, the particle sizes of 100 particles of any thermally conductive filler can be measured using, for example, an electron microscope or an optical microscope, and the average value (arithmetic mean value) can be used as the average particle size. Similarly, the particle size is measured, and the particle size at which the cumulative volume is 100% is defined as D100. When the thermally conductive filler is, for example, an agglomerated particle, the average particle size of the agglomerated particles may be within the above range.
[0097] The thermally conductive filler may be used alone or in combination with two or more types. However, from the viewpoint of effectively improving the heat dissipation properties of the thermal insulation resin sheet, it is preferable to use two or more types with different average particle sizes in combination, and more preferably to use two types with different average particle sizes in combination. The thermally conductive filler preferably includes, for example, a small-particle thermally conductive filler with an average particle size of 0.05 μm or more but less than 1.5 μm and a large-particle thermally conductive filler with an average particle size of 1.5 μm or more but less than 10 μm. The average particle size of the small-particle thermally conductive filler is preferably 0.1 μm or more but less than 1 μm, and the average particle size of the large-particle thermally conductive filler is preferably 2 μm or more but less than 8 μm. When a small-particle-size thermally conductive filler and a large-particle-size thermally conductive filler are used in combination, the ratio of the amount of the large-particle-size thermally conductive filler to the amount of the small-particle-size thermally conductive filler (amount of large-particle-size thermally conductive filler / amount of small-particle-size thermally conductive filler) is, for example, 0.5 to 10, preferably 1 to 5, and more preferably 1.5 to 3. Note that a thermally conductive resin sheet can be determined to contain two or more types of thermally conductive fillers with different average particle sizes when two or more peaks appear in the particle size distribution of the thermally conductive fillers.
[0098] <Epoxy Resin> The thermal insulating resin sheet of the second invention contains an epoxy resin having a mesogenic skeleton. The mesogenic skeleton is a molecular structure that can exhibit liquid crystallinity, which improves alignment after curing and facilitates increasing the thermal conductivity of the cured thermal insulating resin sheet. The epoxy resin having a mesogenic skeleton preferably has two or more epoxy groups per molecule, with the number of epoxy groups per molecule being more preferably 2 to 4, and even more preferably 2. Having two epoxy groups makes it easier to improve alignment after curing, which in turn facilitates increasing thermal conductivity.
[0099] An example of a structure having a mesogenic skeleton is the structure of the following formula (1). In formula (1), * is independently a bond to a group containing an epoxy group or a bond to a linking group bonded to another mesogenic skeleton, k is an integer of 0 to 4, and Y is independently -R, -OR, a halogen atom, -CN, or -NO. 2 , and -COCH 3 R is an aliphatic hydrocarbon group having 1 to 8 carbon atoms. X is at least one selected from the group represented by formula (A) below.
[0100] In group (A), n is an integer of 0 to 4, s is an integer of 0 to 7, m is an integer of 0 to 8, l is an integer of 0 to 12, and r is an integer of 0 to 8. Y is as described above.
[0101] In formula (1), the bonding position indicated by * is preferably the para position relative to X, that is, the structure shown in formula (1) is preferably the following formula (1-1). In formula (1-1), *, X, Y, and k are as described above.
[0102] In formulas (1) and (1-1), Y is preferably a halogen atom or an alkyl group, more preferably an alkyl group. The halogen atom is any of a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. The alkyl group may be linear, branched, or cyclic, but is preferably linear. Specific examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a t-butyl group, an n-pentyl group, an n-hexyl group, and an n-octyl group, and among these, a methyl group is preferred. k is preferably 0 to 2. n is preferably 0 to 2. s is preferably 0 to 5, more preferably 0 to 2. m is preferably 0 to 4, more preferably 0 to 2. l is preferably 0 to 6, more preferably 0 to 3. r is preferably 0 to 4, more preferably 0 to 2, and most preferably 0.
[0103] In formula (1) or formula (1-1), the mesogenic skeleton is preferably a skeleton in which X is a single bond or a group containing —COO—, more preferably a biphenyl skeleton in which X is a single bond or a phenylbenzoate skeleton in which X is —COO—, and among these, a biphenyl skeleton is even more preferable from the viewpoint of improving the alignment after curing and making it easier to impart excellent thermal conductivity to the thermal insulation resin sheet.
[0104] In formulas (1) and (1-1), the epoxy group-containing group bonded to * is preferably an organic group containing an epoxy group having about 2 to 20 carbon atoms, more preferably an organic group containing an epoxy group having 3 to 12 carbon atoms, and even more preferably a group represented by the following formula (2). When the epoxy group-containing group is a group represented by the following formula (2), synthesis of an epoxy resin having a mesogenic skeleton becomes easy.
[0105] In formula (2), * represents a bond to the aromatic ring of the mesogenic skeleton. 1represents a linear or branched alkylene group having 1 to 10 carbon atoms. Examples of the linear or branched alkylene group include a methylene group, a methylmethylene group, a dimethylmethylene group, an ethylene group, a propylene group, a trimethylene group, a tetramethylene group, a pentamethylene group, a hexamethylene group, a heptamethylene group, an octamethylene group, a nonamethylene group, and a decamethylene group. Of these, a methylene group is preferred.
[0106] In addition, it is preferable that in the epoxy resin having a mesogenic skeleton, both * in the above formulas (1) and (1-1) are bonded to a group represented by formula (2). Therefore, the epoxy resin having a mesogenic skeleton preferably has a structure represented by the following formula (1-2). In addition, in formula (1-2), R 1 , X, Y, and k are as described above.
[0107] In the above formulas (1) and (1-1), the linking group bonded to * may be an organic group having about 1 to 24 carbon atoms, preferably an organic group having 3 to 16 carbon atoms, and more preferably an organic group having 4 to 12 carbon atoms. In the above formulas (1) and (1-1), when at least one of * is bonded to a linking group that is bonded to another mesogenic skeleton, the epoxy resin having a mesogenic skeleton will have multiple mesogenic skeletons in one molecule, and in this case, it is preferable that there are two mesogenic skeletons in one molecule. In the above formulas (1) and (1-1), the "another mesogenic skeleton" may be either of the skeletons represented by formulas (1) and (1-1), respectively. The two or more mesogenic skeletons in one molecule may be the same or different, but from the viewpoint of ease of production, they are preferably the same.
[0108] In the above formulas (1) and (1-1), it is also preferable that one of the *'s is bonded to a group containing an epoxy group, and the other * is bonded to a linking group that is linked to another mesogenic skeleton. In this case, the group containing an epoxy group is as described above, and among them, a group represented by formula (2) is preferable. Therefore, it is also preferable that the epoxy resin having a mesogenic skeleton has a structure represented by the following formula (1-3). The structure represented by the following formula (1-3) is a structure represented by R 2 By having a linking group represented by the formula: the thermal conductivity is likely to be improved.
[0109] In the formula (1-3), X, Y, k, and R 1 is as described above. 2 is a divalent organic group, and R 2 The number of carbon atoms in R is, for example, 1 to 24, preferably 2 to 16, and more preferably 3 to 12. 2 More specifically, R is a hydrocarbon group which may have a heteroatom such as an oxygen atom, a nitrogen atom, or a sulfur atom. As the heteroatom, an oxygen atom is preferred, and among these, an oxygen atom constituting an ether bond is preferred. 2 From the viewpoint of ease of synthesis, *-O-R 4 A group represented by —O-* is preferred, where * is a bond to the phenyl ring, and R 4 is an aliphatic hydrocarbon group having 1 to 24 carbon atoms, and is preferably a saturated aliphatic hydrocarbon group. 4 R may be linear, branched, or cyclic, but is preferably linear. 4 The number of carbon atoms in R is, for example, 1 to 24, preferably 2 to 16, more preferably 3 to 12, and even more preferably 6 to 12. 4 is preferably a linear or branched alkylene group. 4Specific examples of the alkyl group include an ethylene group, a propylene group, a tetramethylene group, a pentamethylene group, a hexamethylene group, a heptamethylene group, an octamethylene group, a nonamethylene group, a decamethylene group, an undecamethylene group, a dodecamethylene group, a tridecamethylene group, a tetradecamethylene group, a pentadecamethylene group, a hexadecamethylene group, and a heptadecamethylene group, and among these, an octamethylene group is particularly preferred.
[0110] As the epoxy resin having a mesogenic skeleton, a compound represented by the following formula (2-1) or formula (2-2) is particularly preferred. Among these, the compound represented by formula (2-2) is preferred from the viewpoint of improving thermal conductivity. Furthermore, the compound represented by formula (2-1) is preferred from the viewpoint of ease of production of the epoxy resin.
[0111] In addition, in formula (2-1), R 6 are each independently an alkyl group or a hydrogen atom. The alkyl group is as described above, but is preferably a methyl group.
[0112] In addition, in formula (2-2), R 4 is as above.
[0113] The epoxy resin having a mesogenic skeleton may be in a prepolymer state obtained by reacting a portion of it with a curing agent or the like. In the second invention, the curing agent may be any of a curing agent having a triazine skeleton, a cyanate ester curing agent, and a diamine curing agent, which will be described later, but is not limited to these, and may be any of a phenolic curing agent, an acid anhydride curing agent, a mercaptan curing agent, an imidazole curing agent, etc. In the third invention described later, the curing agent may be the cyanate ester compound in the third invention described later, but is not limited to the cyanate ester compound, and may be any of a phenolic curing agent, an amine curing agent, an acid anhydride curing agent, a mercaptan curing agent, an imidazole curing agent, etc.
[0114] The weight-average molecular weight of the epoxy resin having a mesogenic skeleton is preferably less than 10,000, more preferably 5,000 or less, and even more preferably 3,000 or less. The weight-average molecular weight of the epoxy resin having a mesogenic skeleton is not particularly limited, but may be, for example, 200 or more, preferably 250 or more. The weight-average molecular weight is a weight-average molecular weight measured in terms of polystyrene by gel permeation chromatography (GPC). Tetrahydrofuran is preferably used as an eluent in gel permeation chromatography (GPC) measurements. However, when the molecular weight is low, 1,000 or less, the weight-average molecular weight may be calculated from the structural formula. In the thermal insulation resin sheet, the epoxy resin may undergo a reaction upon curing, but the weight-average molecular weight refers to the weight-average molecular weight of the epoxy resin before curing.
[0115] The epoxy equivalent of the epoxy resin having a mesogenic skeleton is not particularly limited, but is, for example, 100 g / eq or more and 1000 g / eq or less. The epoxy equivalent of the epoxy resin is preferably 120 g / eq or more, more preferably 140 g / eq or more, and is preferably 500 g / eq or less, more preferably 400 g / eq or less. The epoxy equivalent can be measured, for example, according to the method specified in JIS K 7236.
[0116] In the thermal insulation resin sheet, the content of the epoxy resin having a mesogenic skeleton is, for example, 20% by mass or more and 90% by mass or less, preferably 30% by mass or more and 85% by mass or less, more preferably 35% by mass or more and 80% by mass or less, and even more preferably 40% by mass or more and 77% by mass or less, based on the total amount of the components of the thermal insulation resin sheet excluding the thermally conductive filler. The epoxy resin having a mesogenic skeleton may be used alone or in combination of two or more types.
[0117] The thermal insulation resin sheet may contain an epoxy resin without a mesogenic skeleton in addition to the epoxy resin having a mesogenic skeleton. The epoxy resin without a mesogenic skeleton may have one or more epoxy groups, preferably two or more. From the viewpoint of thermal conductivity, the content of the epoxy resin without a mesogenic skeleton is preferably low, for example, less than 100 parts by mass, preferably 50 parts by mass or less, more preferably 30 parts by mass or less, and even more preferably 15 parts by mass or less, per 100 parts by mass of the epoxy resin having a mesogenic skeleton. The lower the content of the epoxy resin without a mesogenic skeleton, the better, and the content may be 0 parts by mass or more. However, it is preferable that the epoxy resin without a mesogenic skeleton is not contained. The thermal insulation resin sheet may also contain a resin other than an epoxy resin, as long as the effect of the present invention is not impaired. Such a resin may be a thermosetting resin or a resin other than a thermosetting resin.
[0118] <Curing Agent> The thermal insulating resin sheet according to the second aspect of the present invention includes at least one curing agent selected from the group consisting of a curing agent having a triazine skeleton, a cyanate ester curing agent, and a diamine curing agent. By using these curing agents in addition to the epoxy resin having a mesogen skeleton, the thermal insulating resin sheet can be imparted with excellent thermal conductivity. A curing agent with a melting point of 40°C or less is preferred. A curing agent with a melting point of 40°C or less not only imparts excellent thermal conductivity as described above, but also improves the sheetability of the thermal insulating resin sheet, making it easier to prevent cracks from occurring when the sheet is wound into a roll, for example. From this perspective, the melting point of the curing agent is more preferably 35°C or less, and even more preferably 30°C or less. The melting point of the curing agent can be measured by DSC.
[0119] From the viewpoint of making it easier to improve the thermal conductivity of the thermal insulation resin sheet, at least one selected from the group consisting of curing agents having a triazine skeleton and cyanate ester curing agents is more preferred, and cyanate ester curing agents are even more preferred, among curing agents having a melting point of 40° C. In addition, detailed explanations of the curing agents having a triazine skeleton, cyanate ester curing agents, and diamine curing agents are as described in detail in the first invention, and therefore will not be repeated here.
[0120] In the second aspect of the present invention, the content of the curing agent is preferably 5 to 95 parts by mass, more preferably 10 to 90 parts by mass, and even more preferably 15 to 80 parts by mass, per 100 parts by mass of the epoxy resin. When the content of the curing agent is equal to or greater than the lower limit, the curing reaction with the epoxy resin proceeds sufficiently, making it easier to obtain a thermal insulating resin sheet with excellent sheetability. When the content of the curing agent is equal to or less than the upper limit, the curing reaction with the epoxy resin proceeds without excessive curing agent content, making it easier to suppress bleed-out of the curing agent. Furthermore, by increasing the amount of epoxy resin having a mesogenic skeleton, it becomes easier to obtain a thermal insulating resin sheet with excellent thermal conductivity.
[0121] (Curing Accelerator) The thermal insulation resin sheet of the second invention may contain a curing accelerator. The inclusion of a curing accelerator can enhance the curing properties of the thermal insulation resin sheet of the second invention. The curing accelerator is not particularly limited, and examples thereof include imidazole-based curing accelerators and tertiary amine-based curing accelerators. Of these, it is preferable to use an imidazole-based curing accelerator. Note that a detailed description of the imidazole-based curing accelerator is the same as that of the first invention, and therefore a detailed description thereof will be omitted. In the second invention, one type of curing accelerator may be used alone, or two or more types may be used in combination.
[0122] The content of the curing accelerator is, for example, 0.3 parts by mass or more and 5 parts by mass or less, preferably 0.5 parts by mass or more and 3 parts by mass or less, and more preferably 0.7 parts by mass or more and 2 parts by mass or less, relative to 100 parts by mass of the total amount of the epoxy resin having a mesogenic skeleton and the curing agent.
[0123] (Coupling Agent) The thermal insulation resin sheet of the second invention may contain a coupling agent. Examples of coupling agents include silane coupling agents and titanium coupling agents, with silane coupling agents being preferred. Any known silane coupling agent may be used without particular limitation. Examples include dimethyldimethoxysilane, 3-acryloxypropyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, vinyltrimethoxysilane, n-decyltrimethoxysilane, 3-isocyanatopropyltriethoxysilane, 3-(2-aminoethyl)aminopropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, glycidoxypropyltrimethoxysilane, and N-phenyl-3-aminopropyltrimethoxysilane. Silane coupling agents may be used alone or in combination. The inclusion of a silane coupling agent in the thermal insulation resin sheet facilitates dispersion of the thermally conductive filler, thereby enabling a high loading of the thermally conductive filler and increasing thermal conductivity. The content of the coupling agent in the heat dissipation insulation resin sheet is, for example, 1 part by mass or more and 25 parts by mass or less, preferably 3 parts by mass or more and 20 parts by mass or less, and more preferably 5 parts by mass or more and 15 parts by mass or less, relative to 100 parts by mass of the total amount of the epoxy resin and the curing agent.
[0124] [Other Components] In addition to the above components, the thermal insulation resin sheet according to the second invention may contain other additives such as a flame retardant, an antioxidant, a tackifier, a plasticizer, a thixotropic agent, a colorant, etc. A solvent may be blended into the thermal insulation resin sheet during its manufacturing process, and it is preferable that some of the blended solvent remains in the thermal insulation resin sheet.
[0125] As described in the manufacturing method below, the thermal insulation resin sheet of the second invention comprises a curable resin composition containing an epoxy resin having a mesogenic skeleton and a curing agent, and may be in an uncured or semi-cured state. When the thermal insulation resin sheet is in an uncured or semi-cured state, it has high adhesion to other members and can be bonded to other members with high adhesive strength.
[0126] [Thickness] In the second invention, the details of the thickness of the heat radiation insulation resin sheet are the same as those described for the resin sheet in the first invention, and therefore description thereof will be omitted.
[0127] [Thermal Conductivity] In the second invention, the thermal conductivity of the heat dissipation insulating resin sheet is preferably 2.5 W / (m·K) or higher. A thermal conductivity of 2.5 W / (m·K) or higher improves heat dissipation. From the perspective of heat dissipation, the thermal conductivity is more preferably 3 W / (m·K) or higher, and even more preferably 3.5 W / (m·K) or higher. As described above, increasing the thermal conductivity improves heat dissipation, and when used as a circuit board or a component-embedded board, it can efficiently dissipate heat generated by electronic components mounted on the circuit board or embedded within the heat dissipation insulating resin sheet. The upper limit of the thermal conductivity of the heat dissipation insulating resin sheet is not particularly limited, but in practice it is, for example, approximately 30 W / (m·K). The thermal conductivity of the heat dissipation insulating resin sheet can be determined as described in the examples below.
[0128] [Laminate] The thermal insulation resin sheet of the second invention may be used in a laminate. The laminate may include a support and a thermal insulation resin sheet provided on the support. Details of the support are as described in the first invention, so a detailed description thereof will be omitted. However, in the second invention, metal foil is also preferred as the support in addition to a film made of a plastic material (resin film).
[0129] In the laminate, a protective film similar to that of the support can be further laminated on the surface of the resin composition layer (heat dissipation insulation resin sheet) that is not bonded to the support (i.e., the surface opposite the support), from the same perspective as in the first invention. The thickness of the protective film is not particularly limited, but is, for example, 1 μm to 40 μm. The heat dissipation insulation resin sheet or laminate can be wound into a roll and stored. If the heat dissipation insulation resin sheet (i.e., the laminate) has a protective film, it can be used by peeling off the protective film.
[0130] (Method for Manufacturing Thermal Insulation Resin Sheet and Laminate) The thermal insulation resin sheet can be obtained by molding a curable resin composition into a sheet. The curable resin composition can be obtained by mixing a thermally conductive filler having a mesogenic skeleton, an epoxy resin, and a curing agent, as well as optional additives such as a resin other than the epoxy resin having a mesogenic skeleton, a curing accelerator, a coupling agent, and other additives. The curable resin composition may also be diluted with a dilution solvent such as an organic solvent. The method for molding the curable resin composition into a sheet is not particularly limited, but is the same as described in the method for molding the resin composition into a sheet in the first invention. As described above, a laminate can be obtained by forming the thermal insulation resin sheet on a support. Furthermore, the sheet-shaped curable resin composition (thermal insulation resin sheet) may be heated, if necessary, to semi-cure it into a B-stage state. The organic solvent used as the dilution solvent is also as described in the first invention.
[0131] (Method of Use of the Thermal Insulation Resin Sheet) The thermal insulation resin sheet may be cured and used in various applications as a cured product. The thermal insulation resin sheet may be laminated in the uncured or semi-cured state onto an adherend such as a metal base plate, other substrates, or electronic components, and then cured to be adhered to the adherend. The thermal insulation resin sheet may be used for various applications requiring heat dissipation, but is preferably used as a thermal insulation resin sheet for electronic devices, and more preferably used in semiconductor devices. The semiconductor device is preferably a power module. Power modules are used, for example, in inverters. Power modules are used, for example, in industrial equipment such as elevators and uninterruptible power supplies (UPS), but their applications are not particularly limited. The thermal insulation resin sheet of the second invention has a high filling rate of thermally conductive filler, high thermal conductivity, and high heat dissipation performance, and therefore is also suitable for use in power modules.
[0132] More specifically, the thermal insulating resin sheet may be used as part of a circuit board or as an encapsulant for electronic components, such as semiconductor chips, embedded therein. That is, the second invention also provides a circuit board including an insulating layer formed from the cured product of the thermal insulating resin sheet. The circuit board is preferably a component-embedded substrate. Component-embedded substrates generally have narrow gaps. However, since the D100 of the thermally conductive filler contained in the thermal insulating resin sheet is small, the thermal insulating resin sheet of the second invention can be suitably applied to component-embedded substrates with narrow gaps. Furthermore, the circuit board is preferably used in a semiconductor chip package. In this case, the semiconductor chip package includes a circuit board and a semiconductor chip mounted on the circuit board.
[0133] Furthermore, as described above, the thermal insulating resin sheet may be used as an encapsulant for electronic components, preferably as an encapsulant included in a semiconductor chip package. In this case, the semiconductor chip package may include a semiconductor chip encapsulated with the thermal insulating resin sheet. An example of a semiconductor chip package is shown in FIG. 1 , where the encapsulation layer 120 is a first insulating layer formed from the thermal insulating resin sheet of the second invention, and the resin layer 130 is a second insulating layer formed from a known resin material or thermally conductive resin composition. An example of a method for encapsulating an electronic component such as a semiconductor chip in the thermal insulating resin sheet using the thermal insulating resin sheet of the second invention as an encapsulant is the same as that described above for the example of the method for encapsulating an electronic component such as a semiconductor chip in the resin sheet using the resin sheet of the first invention as an encapsulant.
[0134] (Third Invention) Hereinafter, the third invention will be described with reference to embodiments. The heat-dissipating resin sheet of the third invention contains an epoxy resin having a mesogenic skeleton and a cyanate ester compound having a melting point of 40° C. or less.
[0135] <Epoxy Resin> The heat-dissipating resin sheet of the third invention contains an epoxy resin having a mesogenic skeleton. Detailed description of the epoxy resin having a mesogenic skeleton is the same as that described in the second invention, and therefore will not be repeated.
[0136] In the heat-dissipating resin sheet of the third invention, the content of the epoxy resin having a mesogenic skeleton is, for example, 15% by mass or more and 80% by mass or less, preferably 25% by mass or more and 75% by mass or less, more preferably 30% by mass or more and 70% by mass or less, and even more preferably 45% by mass or more and 65% by mass or less, based on the total amount of the components of the heat-dissipating resin sheet excluding the inorganic filler described below. The epoxy resin having a mesogenic skeleton may be used alone or in combination of two or more types.
[0137] The heat-dissipating resin sheet may contain an epoxy resin that does not have a mesogenic skeleton in addition to the epoxy resin that has a mesogenic skeleton. Details of the epoxy resin that does not have a mesogenic skeleton and its content are as described in the second invention, so further explanation will be omitted. Furthermore, the heat-dissipating resin sheet may contain a resin other than an epoxy resin as long as the effects of the present invention are not impaired. Such a resin may be a thermosetting resin or a resin other than a thermosetting resin.
[0138] <Cyanate ester compound> The cyanate ester compound contained in the heat-dissipating resin sheet of the third invention has a melting point of 40°C or lower. If the melting point of the cyanate ester exceeds 40°C, the flexibility of the heat-dissipating resin sheet before curing or in a B-stage state decreases, and there is a risk of cracks occurring, for example, when the sheet is wound into a roll. From the viewpoint of improving flexibility at around room temperature, the melting point of the cyanate ester compound is preferably 35°C or lower, more preferably 30°C or lower. The lower limit of the melting point of the cyanate ester compound is not particularly limited, but may be, for example, 0°C or higher. The melting point of the cyanate ester compound can be measured by DSC.
[0139] A cyanate ester compound functions as a curing agent for epoxy resins and is a compound having a cyanate ester group (—OCN). A portion of the cyanate ester group trimers during curing to form a triazine skeleton, which, after curing, forms a molecular structure with high alignment together with the epoxy resin, making it easier to improve thermal conductivity. Furthermore, from the viewpoint of improving curability, it is preferable for the cyanate ester compound to have two or more cyanate ester groups per molecule. From the viewpoint of increasing the alignment of the molecular structure, making it easier to improve thermal conductivity, and from the viewpoint of making it easier to lower the melting point, it is more preferable for the cyanate ester compound to have two cyanate ester groups per molecule.
[0140] The cyanate ester compound preferably has a skeleton containing an aromatic ring, and more preferably has a skeleton containing a phenyl ring. Having a skeleton containing an aromatic ring makes it easier to further improve thermal conductivity after curing. Furthermore, the cyanate ester compound preferably has a cyanate ester group directly bonded to the aromatic ring, and more preferably directly bonded to the phenyl ring. Direct bonding of the cyanate ester group to the aromatic ring makes it easier to increase the reactivity of the cyanate ester group, and trimerization and curing by heating are more likely to proceed.
[0141] The molecular weight of the cyanate ester compound is preferably 500 or less. A molecular weight of 500 or less lowers the melting point, making it easier to improve the flexibility of the heat-dissipating resin sheet before curing or in a B-stage state. The molecular weight of the cyanate ester compound is more preferably 400 or less, and even more preferably 320 or less. The molecular weight of the cyanate ester compound is not particularly limited, but may be, for example, 150 or more, or may be 200 or more.
[0142] The cyanate ester compound is preferably a bisphenol-type cyanate ester. The bisphenol-type cyanate ester preferably has a bisphenol skeleton and a structure in which one cyanate ester group is directly bonded to each phenyl group of the bisphenol skeleton. Examples of the bisphenol-type cyanate ester include bisphenol-type cyanate ester resins such as bisphenol E-type cyanate ester resins and bisphenol F-type cyanate ester resins, and among these, bisphenol E-type cyanate ester resins are preferred. The cyanate ester compounds may be used alone or in combination of two or more.
[0143] The cyanate ester compound is preferably contained in the heat-dissipating resin sheet so that the equivalent ratio (OCN / epoxy group) is 0.25 or more, more preferably 0.3 or more, even more preferably 0.4 or more, and even more preferably 0.6 or more. By adjusting the content of the cyanate ester compound so that the equivalent ratio is a certain level or more, the curing of the heat-dissipating resin sheet can be appropriately promoted by heating or the like. Furthermore, the equivalent ratio is preferably 2.5 or less, more preferably 2.0 or less, even more preferably 1.6 or less, and even more preferably 1.2 or less. By setting the equivalent ratio to the upper limit or less, the epoxy resin having a mesogenic skeleton is appropriately aligned after curing, making it easier to improve thermal conductivity. The equivalent ratio (OCN / epoxy group) referred to here is the ratio of the cyanate ester groups of the cyanate ester compound incorporated into the heat-dissipating resin sheet to the epoxy groups of the epoxy resin incorporated into the heat-dissipating resin sheet. In the case of curing by semi-curing or the like, it is the equivalent ratio before curing.
[0144] The heat-dissipating resin sheet of the third invention may contain a curing agent other than a cyanate ester compound, as long as the effect of the present invention is not significantly impaired. The curing agent other than a cyanate ester compound is a compound that can react with an epoxy resin to cure the epoxy resin. The content of the curing agent other than a cyanate ester compound in the heat-dissipating resin sheet is, for example, less than 50 equivalent %, preferably 30 equivalent % or less, and more preferably 10 equivalent % or less, assuming that the total amount of curing agents contained in the heat-dissipating resin sheet is 100 equivalent %. The heat-dissipating resin sheet of the third invention does not need to contain a curing agent other than a cyanate ester compound, and therefore, the blending amount of the curing agent other than a cyanate ester compound may be 0 equivalent % or more.
[0145] <Inorganic Filler> The heat-dissipating resin sheet of the third invention preferably contains an inorganic filler. The inorganic filler is preferably a thermally conductive filler. By containing an inorganic filler that is a thermally conductive filler, the heat-dissipating resin sheet can be imparted with high thermal conductivity. The inorganic filler may be dispersed in a matrix component that contains a resin component including an epoxy resin having a mesogenic skeleton and a curing agent such as a cyanate ester compound.
[0146] From the viewpoint of increasing the thermal conductivity while ensuring the insulating properties of the thermally conductive resin composition, the thermal conductivity of the insulating inorganic filler is, for example, 10 W / (m·K) or more, preferably 15 W / (m·K) or more, and more preferably 20 W / (m·K) or more. The thermal conductivity of the thermally conductive filler is not particularly limited, but may be, for example, 2000 W / (m·K) or less, or 1000 W / (m·K) or less. The thermal conductivity of the inorganic filler can be measured, for example, by a cyclic heating thermoreflectance method using a thermal microscope manufactured by Bethel Co., Ltd., on a filler cross section machined with a cross-section polisher.
[0147] The inorganic filler preferably has electrical insulation properties, and has an electrical resistivity of, for example, 10 8 It is preferable that the filler has a resistance of Ω·m or more. High electrical insulation properties make it suitable for use in electronic devices such as substrates. Therefore, it is preferable that the inorganic filler is a thermally conductive filler that has electrical insulation properties.
[0148] Examples of inorganic fillers include metals, metal oxides, metal nitrides, metal hydroxides, carbon materials, oxides, nitrides, and carbides other than metals. The inorganic filler may be shaped in any form, such as flakes, spheres, crushed particles, irregular shapes, polyhedral shapes, or fibers, or may be in the form of aggregated particles formed by aggregation of primary particles. For example, boron nitride, which will be described later, is preferably used as aggregated particles. Examples of metals in inorganic fillers include aluminum, copper, and nickel; examples of metal oxides include aluminum oxide (e.g., alumina), magnesium oxide, and zinc oxide; and examples of metal nitrides include aluminum nitride. Examples of metal hydroxides include aluminum hydroxide. Examples of carbon materials include spherical graphite, flake graphite, and carbon fibers. Examples of oxides, nitrides, and carbides other than metals include quartz, boron nitride, and silicon carbide. Among these, from the viewpoint of ensuring electrical insulation, metal oxides, metal nitrides, metal hydroxides, oxides other than metals, nitrides, and carbides are preferred, and metal oxides, metal hydroxides, and nitrides are particularly preferred. Specifically, aluminum oxide, aluminum hydroxide, and boron nitride are more preferred. The inorganic fillers described above may be used alone or in combination of two or more.
[0149] The average particle size of the inorganic filler is preferably 0.1 μm or more and 200 μm or less, more preferably 0.5 μm or more and 150 μm or less, and even more preferably 1 μm or more and 110 μm or less. It is also preferable to use, for example, a small-particle filler having an average particle size of 0.1 μm or more and 5 μm or less in combination with a large-particle filler having an average particle size of more than 5 μm and 200 μm or less. By using inorganic fillers with different average particle sizes, the filling rate of the inorganic filler in the thermally conductive resin sheet can be increased. The average particle size of the inorganic filler can be measured by observation with an electron microscope or the like. More specifically, for example, the particle sizes of 50 particles of any thermally conductive filler can be measured using an electron microscope or optical microscope, and the average particle size (arithmetic mean value) can be used as the average particle size. For example, when the inorganic filler is an agglomerated particle as described above, the average particle size of the agglomerated particles may be within the above range.
[0150] The content of the inorganic filler is not particularly limited, but from the viewpoint of improving heat dissipation, it is, for example, 30% by mass or more, preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 85% by mass or more in the heat-dissipating resin sheet. In the third invention, even if the content of the inorganic filler is high, by using specific components in the epoxy resin and curing agent as described above, it is possible to prevent the flexibility of the heat-dissipating resin sheet from being impaired. Furthermore, the content of the inorganic filler is not particularly limited, but in order to contain a certain amount of epoxy resin and cyanate ester compound, it is sufficient that it be 98% by mass or less, preferably 96% by mass or less, more preferably 95% by mass or less, and even more preferably 93% by mass or less.
[0151] (Curing Accelerator) The heat-dissipating resin sheet of the third invention may contain a curing accelerator. The inclusion of a curing accelerator can enhance the curing properties of the heat-dissipating resin sheet. The curing accelerator is not particularly limited, and examples thereof include imidazole-based curing accelerators and tertiary amine-based curing accelerators. Among these, it is preferable to use an imidazole-based curing accelerator. Since the imidazole-based curing accelerator has been described in detail in the first invention, its description will be omitted. A single curing accelerator may be used, or two or more types may be used in combination. The content of the curing accelerator is, for example, 0.1 to 10 parts by mass, preferably 0.2 to 5 parts by mass, and more preferably 0.5 to 3 parts by mass, relative to 100 parts by mass of the total amount of the epoxy resin having a mesogenic skeleton and the cyanate ester compound.
[0152] (Coupling Agent) The heat-dissipating resin sheet of the third invention may contain a coupling agent. Examples of coupling agents include silane coupling agents and titanium coupling agents, with silane coupling agents being preferred. The content of the coupling agent in the heat-dissipating resin sheet is, for example, 0.1% by mass or more and 10% by mass or less, preferably 0.3% by mass or more and 5% by mass or less, and more preferably 0.5% by mass or more and 3% by mass or less, based on the total amount of the heat-dissipating resin sheet. Other details of the silane coupling agent are as described in the second invention.
[0153] [Other Components] In addition to the above components, the heat-dissipating resin sheet of the third invention may contain other additives such as a flame retardant, an antioxidant, a tackifier, a plasticizer, a thixotropic agent, a colorant, etc. Furthermore, a solvent may be blended into the heat-dissipating resin sheet during its manufacturing process, and it is preferable that a portion of the blended solvent remains in the heat-dissipating resin sheet.
[0154] As described in the manufacturing method below, the heat-dissipating resin sheet of the third invention is made of a curable resin composition containing an epoxy resin having a mesogenic skeleton and a cyanate ester compound, and may be uncured or semi-cured in a B-stage state. When the heat-dissipating resin sheet is in an uncured or B-stage state, it has high adhesion to other members and can be bonded to other members with high adhesive strength.
[0155] [Thickness] The thickness of the heat-dissipating resin sheet is not particularly limited, but is, for example, 10 μm or more and 500 μm or less. A thickness of 10 μm or more ensures a certain level of heat dissipation, while a thickness of 500 μm or less makes it easier to reduce the thickness of electronic devices to which the heat-dissipating resin sheet is applied, such as circuit boards and semiconductor devices. The thickness of the heat-dissipating resin sheet is preferably 80 μm or more, more preferably 100 μm or more, and preferably 400 μm or less, more preferably 260 μm or less.
[0156] [Thermal Conductivity] In the third invention, the thermal conductivity of the heat-dissipating resin sheet is preferably 7 W / (m·K) or more. A thermal conductivity of 7 W / (m·K) or more improves heat dissipation. From the viewpoint of heat dissipation, the thermal conductivity is more preferably 8 W / (m·K) or more, and even more preferably 9 W / (m·K) or more. As described above, increasing the thermal conductivity improves heat dissipation, and when used as a circuit board or a component-embedded board, it can efficiently dissipate heat generated by electronic components mounted on the circuit board or embedded within the heat-dissipating resin sheet. The upper limit of the thermal conductivity of the heat-dissipating resin sheet is not particularly limited, but in practice it is, for example, approximately 30 W / (m·K). The thermal conductivity of the heat-dissipating resin sheet can be determined as described in the examples below.
[0157] (Method for producing a heat-dissipating resin sheet) The heat-dissipating resin sheet can be obtained by molding a curable resin composition into a sheet. The curable resin composition can be obtained by mixing an epoxy resin having a mesogenic skeleton and a cyanate ester compound having a melting point of 40°C or less, as well as optionally blending a resin other than the epoxy resin having a mesogenic skeleton, a curing agent other than the cyanate ester compound, an inorganic filler, a curing accelerator, a coupling agent, and other additives other than these. The curable resin composition may also be diluted with a dilution solvent such as an organic solvent.
[0158] The method for forming the curable resin composition into a sheet is not particularly limited, but is the same as that described in the first invention for forming the resin composition into a sheet.
[0159] (Method of Using the Heat-Dissipating Resin Sheet) The heat-dissipating resin sheet may be cured and used for various purposes as a cured product. The heat-dissipating resin sheet may be laminated to an adherend, such as a metal base plate or other substrate, in the uncured or semi-cured state and cured to adhere to the adherend. Specific uses are as described for the heat-dissipating insulating resin sheet in the second invention. The heat-dissipating resin sheet is preferably used as a sealing material. When used as a sealing material, electronic components may be embedded within the heat-dissipating resin sheet. Specifically, the heat-dissipating resin sheet may be laminated on one side of a support to which electronic components, or electronic components and a substrate, are fixed, thereby embedding the electronic components, or electronic components and a substrate, within the heat-dissipating resin sheet and laminating the heat-dissipating resin sheet on the support. The heat-dissipating resin sheet with the embedded electronic components thus cured by heating may be used, for example, as a component-embedded substrate. The heat-dissipating resin sheet with the embedded electronic components may be peeled from the support, laminated on another member, such as another substrate, and then cured.
[0160] The heating temperature when curing the heat dissipation resin sheet is not particularly limited, but may be, for example, in the range of from 70° C. to 240° C., preferably from 120° C. to 220° C., and more preferably from 160° C. to 200° C. The heating time may be, for example, from 5 minutes to 300 minutes, preferably from 10 minutes to 250 minutes, and more preferably from 15 minutes to 200 minutes. When heating for curing, appropriate pressure may be applied, and for example, the sheet may be heated and cured under pressurized or negative pressure, which makes it easier to bond to other members with high adhesive strength when cured.
[0161] The present invention will be explained in more detail below with reference to examples, but the present invention is not limited to these examples in any way.
[0162] 2, a 170 μm-thick resin sheet 10 obtained by the procedure shown in each Example and Comparative Example was laminated on a 75 μm-thick copper plate 12 having three φ10 μm through-holes 11, and then pressed at 100° C. for 1 hour and then at 200° C. for 1 hour while maintaining a pressure of 1 MPa in a vacuum press to allow curing. After curing was complete, the cross section of the through-holes 11 was photographed with an optical microscope, and the image obtained by the photograph was analyzed with a dispersion measurement system ("Luzex AP" manufactured by Nireco Corporation) to perform the following evaluations.
[0163] (Infiltration into narrow spaces) Infiltration into narrow spaces was evaluated based on the following evaluation criteria. AA: Components of the resin sheet 10 flowed into all three through holes 11. A: Components of the resin sheet 10 flowed into two of the three through holes 11. B: Components of the resin sheet 10 flowed into one of the three through holes 11. C: Components of the resin sheet did not flow into any of the through holes 11. *Here, "flowed into the through holes" means that components of the resin sheet flowed down to the bottom of the through holes.
[0164] (Filler / Resin Separability) The probability (%) of the presence of the thermally conductive filler in regions 1 to 5 shown in FIG. 3 was calculated for each region by the above analysis, and the calculated probability of the presence of the thermally conductive filler was applied to the following formula (1) to calculate a value γ (%) for each region.
[0165] * In formula (1), P n is the probability of existence in region n.
[0166] Then, the filler / resin separation was evaluated based on the following evaluation criteria: A: γ was 3% or less in all regions. C: There was one or more regions where γ exceeded 3%.
[0167] [Thermal Conductivity] The resin sheets obtained by the procedures shown in each Example and Comparative Example were cured by pressing them in a vacuum press at 100°C for 1 hour and then at 200°C for 1 hour while maintaining a pressure of 1 MPa. The thermal conductivity of the cured resin sheets in the thickness direction was measured using a laser flash thermal constant measurement device ("LFA447" manufactured by NETZSCH).
[0168] [Sheet properties] As shown in Fig. 4, a resin sheet 10 having a width of 10 mm and a length of 100 m obtained by the procedure shown in each example and comparative example was wrapped around a metal rod 20 having a diameter of X mm, and cracks were evaluated based on the following evaluation criteria. AA: When X was 3, no cracks occurred in the resin sheet. A: When X was 5, no cracks occurred in the resin sheet. C: When X was 5 or more, cracks occurred in the resin sheet.
[0169] The components used in the examples and comparative examples are as follows.
[0170] (Thermal conductive filler) Alumina 1: "AA03", manufactured by Sumitomo Chemical Co., Ltd., average diameter 0.44 μm, single crystalline α-alumina Alumina 2: "AA05", manufactured by Sumitomo Chemical Co., Ltd., average diameter 0.5 μm, single crystalline α-alumina Alumina 3: "AA1.5", manufactured by Sumitomo Chemical Co., Ltd., average diameter 1.6 μm, single crystalline α-alumina Alumina 4: "AA3", manufactured by Sumitomo Chemical Co., Ltd., average diameter 3.5 μm, single crystalline α-alumina Alumina 5: "AA5", manufactured by Sumitomo Chemical Co., Ltd., average diameter 5.4 μm, single crystalline α-alumina Alumina 6: "AA10", manufactured by Sumitomo Chemical Co., Ltd., average diameter 13.5 μm, single crystalline α-alumina Alumina 7: "AS50", manufactured by Showa Denko K.K., average diameter 9 μm, single crystalline α-alumina Alumina 8: "Y2", manufactured by Ginet Corporation, average diameter 1.9 μm, crushed α-alumina. Alumina 9: "Y4", manufactured by Ginet Corporation, average diameter 3.83 μm, crushed α-alumina. Alumina 10: "YC5", manufactured by Ginet Corporation, average diameter 6.25 μm, crushed α-alumina. Alumina 11: "Y10", manufactured by Ginet Corporation, average diameter 11 μm, crushed α-alumina. Alumina 12: "AO502", manufactured by Admatechs Corporation, average diameter 0.3 μm, polycrystalline θ-alumina. Alumina 13: "AO509", manufactured by Admatechs Corporation, average diameter 10.6 μm, polycrystalline θ-alumina. Alumina 14: "DAW-01DC", manufactured by Denka Corporation, average diameter 1.6 μm, polycrystalline θ-alumina. Alumina 15: "DAW-03DC", manufactured by Denka Corporation, average diameter 3.6 μm, polycrystalline θ-alumina
[0171] Aluminum nitride 1: "HF-01D", manufactured by Tokuyama Corporation, average diameter 1.3 μm, polycrystalline Aluminum nitride 2: "HF-10", manufactured by Tokuyama Corporation, average diameter 7.8 μm, polycrystalline
[0172] Diamond 1: "AGD9", manufactured by Tomei Diamond Co., Ltd., average diameter 9 μm, single crystal Diamond 2: "AGD11", manufactured by Tomei Diamond Co., Ltd., average diameter 11 μm, single crystal
[0173] Silicon carbide 1: "SSC-A01", manufactured by Shinano Electric Smelting Co., Ltd., average diameter 1 μm, polycrystalline Silicon carbide 2: "SSC-A05", manufactured by Shinano Electric Smelting Co., Ltd., average diameter 5 μm, polycrystalline
[0174] (Epoxy Resins) Epoxy Resin 1: "JER828", manufactured by Mitsubishi Chemical Corporation, bisphenol A type epoxy resin, epoxy equivalent 189 g / eq. Epoxy Resin 2: "JER806", manufactured by Mitsubishi Chemical Corporation, bisphenol F type epoxy resin, epoxy equivalent 165 g / eq. Epoxy Resin 3: "YL6121HA", manufactured by Mitsubishi Chemical Corporation, epoxy resin having a mesogen skeleton, epoxy equivalent 175 g / eq. Epoxy Resin 4: "HP7200L", manufactured by DIC Corporation, dicyclopentadiene type epoxy resin, epoxy equivalent 247 g / eq.
[0175] (Curing Agents) Curing agent 1: "P-201", manufactured by Mitsubishi Gas Chemical Co., Ltd., equivalent weight 132 Curing agent 2: "TA", manufactured by Mitsubishi Gas Chemical Co., Ltd., equivalent weight 139 Curing agent 3: "LA-1356", manufactured by DIC Corporation, equivalent weight 146 Curing agent 4: "4,4-diaminodiphenylmethane", manufactured by TCI Corporation, equivalent weight 198 Curing agent 5: "Rikacid MH-700", manufactured by New Japan Chemical Co., Ltd., equivalent weight 164
[0176] (Polymers) Polymer 1: "JER1256", manufactured by Mitsubishi Chemical Corporation, weight average molecular weight 50,000, phenoxy resin Polymer 2: "JER4250", manufactured by Mitsubishi Chemical Corporation, weight average molecular weight 60,000, phenoxy resin Polymer 3: "JER4275", manufactured by Mitsubishi Chemical Corporation, weight average molecular weight 60,000, phenoxy resin Polymer 4: "YX7553BH30", manufactured by Mitsubishi Chemical Corporation, molecular weight 35,000, phenoxy resin Polymer 5: "YP-50S", manufactured by Nippon Steel Chemical & Material Co., Ltd., molecular weight 50,000, phenoxy resin
[0177] (Curing accelerator) Curing accelerator 1: "2PHZ-PW", manufactured by Shikoku Chemical Industry Co., Ltd. Curing accelerator 2: "TPP-MK", manufactured by Hokko Chemical Industry Co., Ltd.
[0178] (Dispersants) Dispersant 1: "KBM573", manufactured by Shin-Etsu Chemical Co., Ltd., a silane coupling agent Dispersant 2: "KBM403", manufactured by Shin-Etsu Chemical Co., Ltd., a silane coupling agent Dispersant 3: "KBM503", manufactured by Shin-Etsu Chemical Co., Ltd., a silane coupling agent Dispersant 4: "KBM3063", manufactured by Shin-Etsu Chemical Co., Ltd., a silane coupling agent Dispersant 5: "DISPER BYK111", manufactured by BYK Japan Dispersant 6: "DISPER BYK145", manufactured by BYK Japan
[0179] [Example 1] A diluted resin composition was obtained by adding the components shown in Table 1 and a solvent, methyl ethyl ketone, so that the solid content was 80% by mass. The diluted resin composition obtained was applied to a support made of a release PET sheet and dried at 90°C for 10 minutes to form a thin film of the resin composition on the release PET sheet, thereby obtaining a resin sheet with a thickness of 100 µm.
[0180] [Examples 2 to 59, Comparative Examples 1 to 15] The same procedures as in Example 1 were carried out except that the formulations were changed as shown in Tables 1 to 8.
[0181]
[0182]
[0183]
[0184]
[0185]
[0186]
[0187]
[0188] *In Tables 1 to 8, the average particle size of the filler is the average particle size of all the thermally conductive fillers contained in the resin sheet.
[0189] As is clear from the above examples, a resin sheet that meets the requirements of the first invention can penetrate into narrow spaces while suppressing separation of the resin and the thermally conductive filler, thereby exhibiting excellent thermal conductivity.
[0190] In contrast, the resin sheet produced in Comparative Example 1 had a lower thermally conductive filler filling rate than specified, resulting in a lower viscosity of the resin sheet and the resin penetrating into narrow spaces first, causing separation between the resin and the thermally conductive filler. The resin sheet produced in Comparative Example 2 was overfilled with thermally conductive filler, causing friction between the thermally conductive fillers, which lost fluidity and caused separation between the resin and the thermally conductive filler. The sheet properties also deteriorated. The resin sheets produced in Comparative Examples 3 to 8 did not contain a single-crystalline filler, causing friction between the thermally conductive fillers and separation between the resin and the thermally conductive filler. The resin sheets produced in Comparative Examples 9 and 10 had a smaller average particle size of the thermally conductive filler than specified, which increased the surface area of the thermally conductive filler, causing friction between the thermally conductive fillers and separation between the resin and the thermally conductive filler. Furthermore, in the resin sheets produced in Comparative Examples 10 to 15, the average particle size of the thermally conductive filler was larger than the specified value, so the thermally conductive filler could not penetrate into narrow spaces, and separation occurred between the resin and the thermally conductive filler.
[0191] (Second Invention) Next, examples and comparative examples of the second invention were carried out as follows.
[0192] [Melting Point] The melting point of a curing agent such as a cyanate ester compound was measured using a differential scanning calorimeter (DSC) (apparatus name "EXTEAR DSC6100", manufactured by SII NanoTechnology Inc.) at a temperature increase rate of 10°C / min. The value measured as the temperature of the endothermic peak was taken as the melting point. [Evaluation of Sheet Properties] The thermal insulating resin sheets obtained in each Example and Comparative Example, each 200 mm wide and 300 m long, were wrapped around a cylindrical core with a diameter of 90 mm in an environment of 25°C, and the sheet properties were evaluated based on the presence or absence of cracks. Sheets that did not generate cracks were rated "A", and sheets that generated cracks were rated "B".
[0193] [Thermal Conductivity] The resin sheets (heat dissipation insulating resin sheets) obtained in each Example and Comparative Example were cured and their thermal conductivity was measured using the same method as in the Example of the first invention. Thermal conductivity of 3.0 W / (m K) or more was evaluated as "A," 2.5 W / (m K) or more but less than 3.0 W / (m K) was evaluated as "B," and less than 2.5 W / (m K) was evaluated as "C."
[0194] The components used in the examples and comparative examples of the second invention are as follows: (Epoxy resin) Epoxy A: an epoxy resin having a mesogenic skeleton of the following structure, molecular weight 682 Epoxy B: "YL6121HA", manufactured by Mitsubishi Chemical Corporation, an epoxy resin having a mesogen skeleton with the following structure, molecular weight 326 Epoxy C: "YD-127", manufactured by Nippon Steel Chemical Co., Ltd., bisphenol A type epoxy resin
[0195] (Curing agent) Cyanate A: "P-201" manufactured by Mitsubishi Gas Chemical Company, Inc., a cyanate ester-based curing agent having the following structure, molecular weight 264, melting point: 29°C Cyanate B: "TA", manufactured by Mitsubishi Gas Chemical Company, Inc., cyanate ester curing agent having the following structure, molecular weight 278, melting point: 80°C Curing agent having a triazine skeleton: "LA-1356", manufactured by DIC Corporation, a curing agent having the following structure Diamine curing agent: "DDM", manufactured by TCI, 4,4-diaminodiphenylmethane, molecular weight 198, melting point: 91°C Acid anhydride: "Rikacid MH-700", manufactured by New Japan Chemical Co., Ltd., a mixture of 4-methylhexahydrophthalic anhydride and hexahydrophthalic anhydride
[0196] Curing accelerator: "2PHZ-PW", manufactured by Shikoku Chemical Industry Co., Ltd. Coupling agent: "KBM-573", manufactured by Shin-Etsu Chemical Co., Ltd., N-phenyl-3-aminopropyltrimethoxysilane
[0197] (Thermal conductivity filler) Alumina 1: "AA-03", manufactured by Sumitomo Chemical Co., Ltd., polyhedral alumina, average particle size 0.3 μm, maximum particle size (D100) less than 10 μm Alumina 2: "AA-3", manufactured by Sumitomo Chemical Co., Ltd., polyhedral alumina, average particle size 3 μm, maximum particle size (D100) less than 10 μm Silica: "Admafine (registered trademark) SO-C2", manufactured by Admatechs Co., Ltd., average particle size 0.5 μm, maximum particle size (D100) less than 10 μm
[0198] Examples 60 to 65, Comparative Examples 16 to 18 The same procedures as in Example 1 were carried out except that the formulation was changed as shown in Table 9.
[0199]
[0200] As is clear from the above examples, the thermal insulation resin sheets satisfying the requirements of the second invention had excellent thermally conductive fillers. In contrast, the resin sheet prepared in Comparative Example 16 did not contain an epoxy resin having a mesogenic skeleton, and the thermal conductivity of the resin sheet was not sufficiently improved. Furthermore, the resin sheet prepared in Comparative Example 17 used a curing agent that was not a triazine-based curing agent, a cyanate ester-based curing agent, or a diamine curing agent, and therefore the thermal conductivity of the resin sheet was not sufficiently improved. Furthermore, the resin sheet prepared in Comparative Example 18 used silica as a filler, which has a thermal conductivity of less than 20 W / m·K, and therefore the thermal conductivity of the resin sheet was not sufficiently improved.
[0201] (Third Invention) Next, the examples and comparative examples of the third invention were carried out as follows. [Melting point] Measured as described in the examples of the second invention. [Sheet property evaluation] The sheet property of the 200 mm wide, 300 m long heat dissipation resin sheets obtained in each example and comparative example was evaluated using the same method as for the heat dissipation and insulation resin sheets of the second invention. [Thermal conductivity] The heat dissipation and insulation resin sheets obtained in each example and comparative example were cured and their thermal conductivity was measured using the same method as for the examples of the first and second inventions. Thermal conductivity of 7 W / (m K) or more was rated "A", and thermal conductivity of less than 7 W / (m K) was rated "B".
[0202] The components used in the examples and comparative examples of the third invention were the same as those of the second invention, except for the following: Alumina 3: "AA-18", manufactured by Sumitomo Chemical Co., Ltd., polyhedral alumina, average particle size 18 μm
[0203] Examples 66 to 69, Comparative Examples 19 to 21 The same procedures as in Example 1 were carried out except that the formulation was changed as shown in Table 10.
[0204]
[0205] As shown in Examples 66 to 69 above, the heat-dissipating resin sheets of each Example contained an epoxy resin having a mesogenic skeleton and a cyanate ester compound having a melting point of 40°C or less, and therefore were able to maintain high thermal conductivity while also achieving good flexibility. In contrast, Comparative Example 19 contained an epoxy resin having a mesogenic skeleton and a cyanate ester compound, and therefore was able to achieve high thermal conductivity, but was unable to achieve good flexibility because the melting point of the cyanate ester compound was higher than 40°C. Furthermore, Comparative Examples 20 and 21 did not contain either an epoxy resin having a mesogenic skeleton or a cyanate ester compound, and therefore were unable to achieve sufficiently high thermal conductivity.
[0206] REFERENCE SIGNS LIST 100 Semiconductor chip package 110 Semiconductor chip 120 Sealing layer (first insulating layer) 130 Rewiring formation layer (insulating layer, second insulating layer) 140 Conductor layer (rewiring layer) 150 Solder resist layer 160 Bump 10 Resin sheet 11 Through hole 12 Copper plate 1 to 5 Region 20 Metal rod
Claims
1. A resin sheet containing a resin and a thermally conductive filler, the resin sheet satisfying the following conditions (1) to (3): (1) The content of the thermally conductive filler is 50% by volume or more and 80% by volume or less based on the total amount of the resin sheet. (2) The average particle size of the thermally conductive filler is 2 μm or more and 8 μm or less. (3) The thermally conductive filler contains a single crystal filler in an amount of 12% by volume or more based on the total amount of the thermally conductive filler.
2. The resin sheet according to claim 1, wherein the resin is a thermosetting resin.
3. The resin sheet according to claim 2, wherein the thermosetting resin comprises an epoxy resin.
4. The resin sheet according to any one of claims 1 to 3, wherein the monocrystalline filler contains alpha alumina.
5. The resin sheet according to any one of claims 1 to 4, wherein the thermally conductive filler is surface-treated with a silane coupling agent, or the resin sheet contains a dispersing agent.
6. A heat dissipation member formed from the resin sheet according to any one of claims 1 to 5.
7. A heat dissipation insulation resin sheet comprising an epoxy resin having a mesogen skeleton, a curing agent, and a thermally conductive filler, wherein the curing agent is at least one selected from the group consisting of curing agents having a triazine skeleton, cyanate ester curing agents, and diamine curing agents, the thermal conductivity of the thermally conductive filler is 20 W / m·K or more, the D100 of the thermally conductive filler is 10 μm or less, and the thermally conductive filler does not contain a thermally conductive filler having a D100 exceeding 10 μm, and the content of the thermally conductive filler is 55 vol% or more and 81 vol% or less, when the non-volatile components in the resin composition constituting the heat dissipation insulation resin sheet are taken as 100 vol%.
8. The thermal insulation resin sheet according to claim 7, wherein the curing agent has a melting point of 40° C. or less.
9. The thermal insulation resin sheet according to claim 8, wherein the curing agent having a melting point of 40° C. or less is at least one selected from the group consisting of curing agents having a triazine skeleton and cyanate ester curing agents.
10. The thermal insulation resin sheet according to claim 8 or 9, wherein the curing agent having a melting point of 40° C. or less is a cyanate ester curing agent.
11. The thermal insulation resin sheet according to any one of claims 7 to 10, wherein the cyanate ester curing agent has a skeleton containing an aromatic ring.
12. The thermal insulation resin sheet according to any one of claims 7 to 11, wherein the molecular weight of the cyanate ester curing agent is 500 or less.
13. The thermal insulation resin sheet according to any one of claims 7 to 12, wherein the epoxy resin has a biphenyl skeleton.
14. The thermal insulation resin sheet according to any one of claims 7 to 13, wherein the diamine curing agent has a molecular weight of 500 or less and is selected from the group consisting of aromatic compounds and alicyclic compounds.
15. A laminate comprising a support and the resin sheet according to any one of claims 1 to 5 and 7 to 14 provided on the support.
16. A circuit board comprising an insulating layer formed from a cured product of the resin sheet according to any one of claims 1 to 5 and 7 to 14.
17. A semiconductor chip package comprising the circuit board according to claim 16 and a semiconductor chip mounted on the circuit board.
18. A semiconductor chip package comprising a semiconductor chip sealed with the resin sheet according to any one of claims 1 to 5 and 7 to 14.
19. A heat dissipating resin sheet comprising an epoxy resin having a mesogenic skeleton and a cyanate ester compound having a melting point of 40° C. or less.
20. The heat dissipating resin sheet according to claim 19, wherein the cyanate ester compound has a skeleton containing an aromatic ring.
21. The heat dissipating resin sheet according to claim 19, wherein the molecular weight of the cyanate ester compound is 500 or less.
22. The heat dissipating resin sheet according to claim 19, wherein the epoxy resin has a biphenyl skeleton.
23. The heat dissipating resin sheet according to claim 19, which contains an inorganic filler.
24. A cured product of the heat dissipation resin sheet according to any one of claims 19 to 23.
25. A resin composition comprising a resin and a thermally conductive filler, the resin composition satisfying the following conditions (1) to (3): (1) The content of the thermally conductive filler is 50% by volume or more and 80% by volume or less based on the total amount of the resin composition. (2) The average particle size of the thermally conductive filler is 2 μm or more and 8 μm or less. (3) The thermally conductive filler contains a single crystal filler in an amount of 12% by volume or more based on the total amount of the thermally conductive filler.
Citation Information
Patent Citations
Insulation film, metal base substrate and metal base substrate production method
JP2021152102A
Epoxy resin composition, composition for electronic component and material for electronic component
JP2022008158A
Epoxy resin composition, heat conductive material precursor, b-stage sheet, prepreg, heat dissipation material, laminated plate, metal substrate, and printed wiring board
WO2017122350A1
Alumina particles and resin composition using same
WO2022255226A1
Cited By
Resin composition, resin sheet, multilayer body, and semiconductor element
WO2026014460A1
Sealing film laminate and electronic component device
WO2026182028A1