Composition, undercoat layer, electrode, and lithium-ion secondary battery
The use of a composition with a conductive carbon material, olefin resin, and acrylic water-soluble polymer in the undercoat layer addresses the challenges of initial DC resistance and high-temperature resistance in lithium-ion secondary batteries, enhancing safety and performance.
Patent Information
- Application Number
- PCT/JP2024/019608
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-05-28
- Publication Date
- 2024-10-03
AI Technical Summary
Lithium-ion secondary batteries face challenges in maintaining safety and performance, particularly in suppressing initial DC resistance during charging and discharging, and the increase in DC resistance over time, especially in high-temperature environments.
A composition comprising a conductive carbon material, an olefin resin, and an acrylic water-soluble polymer, with specific structural units and ratios, is used to form an undercoat layer that reduces initial DC resistance and prevents increases in high-temperature environments, enhancing both safety and battery performance.
The solution effectively stabilizes lithium-ion secondary batteries by reducing initial DC resistance and preventing resistance increases in high-temperature environments, thereby improving safety and maintaining battery performance.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Composition, undercoat layer, electrode, lithium ion secondary battery
[0001] The present disclosure relates to a composition, an undercoat layer, an electrode, and a lithium ion secondary battery.
[0002] In recent years, lithium-ion secondary batteries have been widely used as power sources for electronic devices, electric vehicles, and electrical storage. In particular, there has been a recent demand for batteries with high capacity, high output, and high energy density that can be installed in hybrid vehicles and the like. Such lithium-ion secondary batteries have the advantage of high energy density. However, the use of lithium metal and lithium ions requires adequate safety measures.
[0003] Patent Document 1 discloses a positive electrode for a lithium ion secondary battery that improves the safety of the lithium ion secondary battery. The positive electrode disclosed in Patent Document 1 includes a positive electrode current collector and a positive electrode mixture layer. The positive electrode mixture layer is laminated on at least one side of the positive electrode current collector. The positive electrode mixture layer includes a positive electrode mixture layer and an undercoat layer. The undercoat layer is formed between the positive electrode current collector and the positive electrode mixture layer. The undercoat layer includes a conductive additive, a binder, and thermally expandable microcapsules. The thermally expandable microcapsules have a maximum volume expansion temperature of 70°C to 180°C.
[0004] Patent Document 2 discloses a secondary battery that includes an intermediate layer between a positive electrode current collector and a positive electrode composite layer, the intermediate layer containing a cured product of a curable resin having a specific functional group and a conductive material, in order to suppress an increase in battery temperature when an internal short circuit occurs.
[0005] Patent Document 1: International Publication No. 2019 / 189866 Patent Document 2: International Publication No. 2018 / 198689
[0006] There is a demand for a lithium-ion secondary battery that is not only excellent in safety but also excellent in battery performance, in which DC resistance at the initial stage of charge / discharge and an increase in DC resistance after long-term storage of the lithium-ion secondary battery in a high-temperature environment are suppressed. The output of a lithium-ion secondary battery in which DC resistance at the initial stage of charge / discharge is suppressed is superior to the output of a lithium-ion secondary battery in which DC resistance at the initial stage of charge / discharge is not suppressed. The life of a lithium-ion secondary battery in which an increase in DC resistance after long-term storage in a high-temperature environment is suppressed is superior to the life of a lithium-ion secondary battery in which an increase in DC resistance after long-term storage in a high-temperature environment is not suppressed.
[0007] The problem to be solved by one embodiment of the present disclosure is to provide a composition (preferably an undercoat composition) and an undercoat layer suitable for forming an electrode that is highly safe, has low DC resistance during initial charge and discharge, and exhibits a suppressed increase in DC resistance under high-temperature environments (particularly after long-term storage).The problem to be solved by another embodiment of the present disclosure is to provide an electrode and a lithium-ion secondary battery that are highly safe, have low DC resistance during initial charge and discharge, and exhibits a suppressed increase in DC resistance under high-temperature environments (particularly after long-term storage), and can stably provide excellent battery performance.
[0008] Specific means for solving the problems include the following aspects: <1> A composition comprising a conductive carbon material (A), an olefin resin (B), and an acrylic water-soluble polymer (C), wherein the acrylic water-soluble polymer (C) has structural units derived from (meth)acrylamide and structural units derived from a vinyl monomer having at least one of a carboxy group and a hydroxyl group, the content of the structural units derived from (meth)acrylamide being 35% by mass to 95% by mass relative to the total amount of the acrylic water-soluble polymer (C), and the content of the structural units derived from the vinyl monomer having at least one of a carboxy group and a hydroxyl group being 5% by mass to 65% by mass relative to the total amount of the acrylic water-soluble polymer (C). <2> The composition according to <1>, wherein the content of the conductive carbon material (A) is 1% by mass to 30% by mass, relative to the total amount of the composition, the content of the olefin-based resin (B) is 30% by mass to 90% by mass, relative to the total amount of the composition, and the content of the acrylic water-soluble polymer (C) is 1% by mass to 20% by mass, relative to the total amount of the composition. <3> The composition according to <1> or <2>, wherein the olefin-based resin (B) comprises an ethylene-based resin or a propylene-based resin. <4> The composition according to any one of <1> to <3>, wherein the particle size of the olefin-based resin (B) is 0.1 μm to 9.0 μm, and the softening point of the olefin-based resin (B) is 70°C or higher. <5> The composition according to any one of <1> to <4>, wherein the acrylic water-soluble polymer (C) has a structural unit derived from (meth)acrylamide, a structural unit derived from a vinyl monomer having a carboxy group, and a structural unit derived from a vinyl monomer having a hydroxyl group. <6> The composition according to any one of <1> to <5>, wherein the acrylic water-soluble polymer (C) has a Tg of 150° C. or higher. <7> The composition according to any one of <1> to <6>, further comprising an additive (D), wherein the content of the additive (D) is 1% by mass to 50% by mass relative to the total amount of the composition. <8> The composition according to <7>, wherein the additive (D) includes carboxymethyl cellulose.<9> The composition according to <7> or <8>, wherein the additive (D) comprises at least one of a thermally expandable microcapsule having a maximum volume expansion temperature of 70°C to 180°C and an inorganic oxide filler. <10> The composition according to any one of <1> to <9>, wherein the ratio of particle size distribution D99 to particle size distribution D10 (D99 / D10), measured by a laser light diffraction scattering method, is 35 or less. <11> The composition according to any one of <1> to <10>, wherein the particle size distribution D99, measured by a laser light diffraction scattering method, is 20 μm or less. <12> The composition according to any one of <1> to <11>, wherein the ratio of particle size distribution D99 to particle size distribution D50 (D99 / D50), measured by a laser light diffraction scattering method, is 20 or less. <13> An undercoat layer comprising the composition according to any one of <1> to <12>. <14> An electrode comprising a current collector, the undercoat layer according to <13>, and a composite layer. <15> The electrode according to <14>, in which the current collector, the undercoat layer, and the composite layer are laminated in this order. <16> A lithium ion secondary battery comprising the electrode according to <14> or <15>.
[0009] According to the present disclosure, a composition (preferably an undercoat composition) and an undercoat layer suitable for forming an electrode that is highly safe, has low DC resistance during initial charge and discharge, and exhibits a suppressed increase in DC resistance under high-temperature environments (particularly after long-term storage) are provided. Also, according to another embodiment of the present disclosure, an electrode and a lithium-ion secondary battery are provided that are highly safe, have low DC resistance during initial charge and discharge, and exhibit a suppressed increase in DC resistance under high-temperature environments (particularly after long-term storage), and can stably provide excellent battery performance.
[0010] Fig. 1 is a schematic cross-sectional view showing a laminated battery as an example of the lithium ion secondary battery of the present disclosure. Fig. 2 is a schematic cross-sectional view of a positive electrode in a lithium ion secondary battery according to an embodiment of the present disclosure. Fig. 3 is a schematic cross-sectional view of a negative electrode in a lithium ion secondary battery according to an embodiment of the present disclosure. Fig. 4 is a schematic side view showing an example of a three-roll mill.
[0011] The present disclosure will be described in detail below. The following description of the components may be based on representative embodiments of the present disclosure, but the present disclosure is not limited to such embodiments.
[0012] In the present disclosure, a numerical range indicated using "to" indicates a range that includes the numerical value before "to" as the lower limit and the numerical value before "to" as the upper limit. In the numerical ranges described in stages in the present disclosure, the upper limit or lower limit described in a certain numerical range may be replaced with the upper limit or lower limit of another numerical range described in stages. Furthermore, in the numerical ranges described in the present disclosure, the upper limit or lower limit described in a certain numerical range may be replaced with a value shown in the examples.
[0013] In the description of groups (atomic groups) in this specification, when a notation does not specify whether the group is substituted or unsubstituted, it encompasses both unsubstituted groups (atomic groups) and substituted groups (atomic groups). For example, the term "alkyl group" encompasses not only unsubstituted alkyl groups (unsubstituted alkyl groups) but also substituted alkyl groups (substituted alkyl groups).
[0014] In this specification, "(meth)acrylate" refers to either or both of acrylate and methacrylate, "(meth)acrylic" refers to either or both of acrylic and methacrylic, and "(meth)acryloyl" refers to either or both of acryloyl and methacryloyl.
[0015] In this specification, the term "step" refers not only to an independent step, but also to a step that cannot be clearly distinguished from other steps, as long as the intended effect of the step is achieved. The present disclosure will be described in detail below.
[0016] (1) Composition The composition of the present disclosure contains a conductive carbon material (A), an olefin resin (B), and an acrylic water-soluble polymer (C). The acrylic water-soluble polymer (C) has structural units derived from (meth)acrylamide and structural units derived from a vinyl monomer having at least one of a carboxy group and a hydroxyl group. The content of the structural units derived from (meth)acrylamide is 35% by mass to 95% by mass, based on the total amount of the acrylic water-soluble polymer (C). The content of the structural units derived from the vinyl monomer having at least one of a carboxy group and a hydroxyl group is 5% by mass to 65% by mass, based on the total amount of the acrylic water-soluble polymer (C).
[0017] In this disclosure, the term "conductive carbon material" refers to a carbon material having a volume resistivity at 20°C of less than 40 Ω·cm, preferably less than 3 Ω·cm. In this disclosure, the term "olefin-based resin" refers to a resin containing structural units derived from an olefin. Specifically, "olefin-based resin" includes olefin homopolymers, copolymers of two or more olefins, and copolymers of olefins and other monomers. In this disclosure, the term "acrylic water-soluble polymer" refers to a polymer containing structural units derived from a monomer having a (meth)acryloyl group (hereinafter also referred to as "(meth)acrylic monomer"). The term "acrylic water-soluble polymer" includes homopolymers of (meth)acrylic monomers and copolymers of two or more (meth)acrylic monomers. In this disclosure, the term "water-soluble polymer" refers to a polymer that has a residual solid content of 0.1% or less when 1 g of the polymer is dissolved in 100 ml of water by stirring for 24 hours and then filtered through a 300-mesh wire screen. In this disclosure, the terms "content" and "addition amount" are considered to be substantially the same.
[0018] The composition of the present disclosure has the above-described configuration, and therefore can form an electrode that is excellent in safety, has low DC resistance during initial charge / discharge, and suppresses an increase in DC resistance under high-temperature environments (particularly after long-term storage). In other words, when the composition of the present disclosure is applied to a secondary battery including an electrode, a lithium-ion secondary battery can be obtained that has a good balance between safety and battery performance (i.e., output and life).
[0019] The reason why the present disclosure exhibits its effects is not entirely clear, but is presumed to be as follows. Among the resin components contained in the composition of the present disclosure, the water-dispersible olefin resin (B) melts at a lower temperature range. In other words, it is advantageous for exhibiting a shutdown function during heat generation. The acrylic water-soluble polymer (C) contains (meth)acrylamide, which has excellent heat resistance. As a result, when the composition of the present disclosure is used as a raw material for an undercoat layer, the heat resistance, electrolyte resistance, and ion permeability of the undercoat layer are improved in a balanced manner. Therefore, an electrode is obtained that is excellent in safety, and not only has low DC resistance during initial charge and discharge, but also significantly suppresses an increase in DC resistance under high-temperature environments (especially after long-term storage). As a result, when a lithium secondary battery is fabricated using the composition of the present disclosure, it becomes a lithium-ion secondary battery that has a good balance between safety and battery performance (i.e., output and life).
[0020] The composition of the present disclosure is suitable for use in, for example, electrode components of lithium-ion secondary batteries. Specifically, the composition of the present disclosure is preferably used to form an undercoat layer included in a lithium-ion secondary battery including an electrode in which an undercoat layer and a composite layer are laminated in this order on at least one main surface of a current collector. In particular, the composition of the present disclosure is more preferably used to form an undercoat layer included in a positive electrode in a lithium-ion secondary battery including a positive electrode in which an undercoat layer and a composite layer are laminated in this order on at least one main surface of a current collector.
[0021] In this disclosure, the term "current collector" refers to a sheet-like object that collects electrons generated from an active material in a lithium-ion secondary battery and supplies the electrons to the active material. The term "main surfaces of the current collector" refers to a pair of opposing surfaces with the largest area among multiple pairs of opposing surfaces.
[0022] (1.1) Conductive Carbon Material (A) The composition of the present disclosure contains a conductive carbon material (A), which reduces the electrical resistance of the composition of the present disclosure.
[0023] Examples of the conductive carbon material (A) include graphite, carbon black, conductive carbon fiber, and fullerene. Examples of graphite include artificial graphite and natural graphite (e.g., flake graphite, lump graphite, and amorphous graphite). Examples of the conductive carbon fiber (A) include carbon nanotubes, carbon nanofibers, and carbon fibers. The conductive carbon material (A) may be used alone or in combination of two or more.
[0024] The shape of the conductive carbon material (A) is not particularly limited and may be particulate. When the conductive carbon material (A) is particulate, the particle size of the conductive carbon material (A) is not particularly limited. From the viewpoint of dispersing the conductive carbon material (A) among the particles contained in the undercoat layer and functioning as a conductive assistant, the particle size of the conductive carbon material (A) is preferably 5 μm or less, more preferably 1 μm to 4 μm. In this case, the primary particle size of the particles of the conductive carbon material is preferably 0.5 μm or less, more preferably 0.1 μm to 0.4 μm. The particle size of the conductive carbon material (A) indicates a particle size (particle size distribution D50, median diameter) corresponding to a cumulative 50% by volume from the fine particle side in a volume-based particle size distribution measured using a particle size distribution measuring device based on a laser light diffraction scattering method.
[0025] The conductive carbon material (A) may be a commercially available product. Examples of commercially available carbon black include "Super P" (manufactured by TIMCAL). Examples of commercially available flake graphite include "KS-6" (manufactured by TIMREX).
[0026] The content of the conductive carbon material (A) is not particularly limited and is preferably 1% by mass to 30% by mass relative to the total amount of the composition. When the content of the conductive carbon material (A) is within the above range, the number of contact points between the conductive carbon materials (A) in the composition of the present disclosure is large, and the electrical resistance of the composition of the present disclosure at room temperature can be reduced by the percolation effect. Furthermore, when the temperature of the lithium ion secondary battery rises suddenly, contact between the conductive carbon materials (A) is difficult to maintain, and the electrical resistance of the undercoat layer increases, allowing the resulting lithium ion secondary battery to exhibit a shutdown function. In other words, the safety of the lithium ion secondary battery is excellent. The shutdown function includes preventing the progress of the battery reaction of the lithium ion secondary battery. The "battery reaction" refers to the insertion and desorption reactions of lithium ions that occur between the positive electrode and the negative electrode. The higher the content of the conductive carbon material (A), the better the battery performance of the lithium ion secondary battery tends to be. From the viewpoint of ensuring the shutdown function, the content of the conductive carbon material (A) is preferably 28% by mass or less, more preferably 25% by mass or less, and even more preferably 20% by mass or less, relative to the total amount of the composition. From the viewpoint of ensuring the battery performance, the content of the conductive carbon material (A) is preferably 3% by mass or more, more preferably 5% by mass or more, and even more preferably 10% by mass or more, relative to the total amount of the composition.
[0027] (1.2) Olefin-Based Resin (B) The composition of the present disclosure contains an olefin-based resin (B). As a result, when the composition of the present disclosure is used as a raw material for the undercoat layer, the lithium ion secondary battery is less susceptible to thermal runaway, and the safety of the lithium ion secondary battery is further improved.
[0028] The material of the olefin resin (B) is not particularly limited. The softening point of the olefin resin (B) is preferably 150°C or lower, more preferably 140°C or lower, and even more preferably 135°C or lower, from the viewpoint of more effectively exerting the shutdown function by melting the olefin resin (B) in a lower temperature range during a sudden temperature rise of the lithium ion secondary battery (hereinafter referred to as "effective exertion of the shutdown function"). The softening point of the olefin resin (B) is preferably 70°C or higher, more preferably 90°C or higher, even more preferably 110°C or higher, and particularly preferably 120°C or higher, from the viewpoint of maintaining the shape of the olefin resin (B) before and after the drying treatment performed in the manufacturing process of the positive electrode (hereinafter referred to as "shape maintenance of the olefin resin (B) during the positive electrode drying process"). The softening point of the olefin resin (B) is preferably 70°C to 150°C. The softening point of the olefin resin (B) is a value measured by JIS K2207 (ring and ball method).
[0029] Examples of the olefin resin (B) include ethylene resins (e.g., polyethylene, ethylene-vinyl acetate copolymer (EVA), or polyethylene oxide), propylene resins (e.g., polypropylene), polyvinyl chloride, polyvinylidene chloride, polyvinyl fluoride, polyvinylidene fluoride, polyamide, polystyrene, polyacrylonitrile, and polymethyl (meth)acrylate. Among these, the olefin resin (B) preferably contains an ethylene resin or a propylene resin, from the viewpoint of achieving both effective shutdown function and shape retention of the olefin resin during the positive electrode drying step.
[0030] An "ethylene-based resin" is a resin containing ethylene as a main component, and a "propylene-based resin" is a resin containing propylene as a main component. Here, "main component" refers to the component contained in the resin with the largest content. Examples of ethylene-based resins include homopolymers and copolymers of ethylene. Of these, the ethylene-based resin is preferably a copolymer of ethylene and at least one α-olefin. Examples of propylene-based resins include homopolymers and copolymers of propylene.
[0031] The olefin resin (B) preferably contains a water-dispersible olefin resin, which makes the lithium ion secondary battery less susceptible to thermal runaway when the composition of the present disclosure is used as a raw material for the undercoat layer, thereby improving the safety of the lithium ion secondary battery.
[0032] In the present disclosure, the term "water-dispersible olefin-based resin" refers to an olefin-based resin that can be dispersed in water without the addition of at least one of a surfactant and an organic solvent.
[0033] Examples of the water-dispersible olefin resin material include polyethylene, polyethylene elastomer, polyolefin ionomer, and EVA.
[0034] The content of the water-dispersible olefin resin is not particularly limited, and is preferably 20% by mass or more, more preferably 50% by mass or more, and may be 100% by mass, based on the total amount of the olefin resin (B).
[0035] As the olefin-based resin (B), commercially available products on the market may be used. Commercially available olefin-based resin (B) products include the Chemipearl (registered trademark) series (aqueous polyolefin dispersions) manufactured by Mitsui Chemicals, Inc. Examples of finely particulate aqueous dispersions of polyethylene or polypropylene include WP100, W100, W200, W300, W308, W310, W400, W401, W410, W4005, W500, WF640, W700, W800, W900, W950, P301W, and WH201.
[0036] The shape of the olefin-based resin (B) is not particularly limited and may be particulate. When the olefin-based resin (B) is particulate, the particle size is not particularly limited. From the viewpoint of adjusting the particle size of the olefin-based resin so that it falls within the optimal film thickness range of the undercoat layer, the particle size of the olefin-based resin (B) is preferably 9.0 μm or less, more preferably 4.0 μm or less, and even more preferably 2.0 μm or less, as an average primary particle size. From the viewpoint of processability of the composition (e.g., slurry for the undercoat layer), the particle size of the olefin-based resin (B) is preferably 0.1 μm or more, more preferably 0.5 μm or more. The particle size of the olefin-based resin (B) is preferably 0.1 μm to 9.0 μm. The smaller the particle size of the olefin-based resin (B), the more likely the olefin-based resin (B) is to aggregate. The particle size of the olefin-based resin (B) is the average primary particle size measured by a Cole counter method.
[0037] The particle size of the olefin-based resin (B) is preferably 0.1 μm to 9.0 μm, and the softening point of the olefin-based resin (B) is preferably 70° C. or higher. As a result, when the composition of the present disclosure is used as a raw material for the undercoat layer, the lithium ion secondary battery is less susceptible to thermal runaway, and the safety of the lithium ion secondary battery is further improved.
[0038] The olefin resin (B) may be used alone or in combination of two or more. The content of the olefin resin (B) is preferably 30% to 90% by mass relative to the total amount of the composition. When the content of the olefin resin (B) is within the above range, the shutdown function can be well ensured. The higher the content of the olefin resin (B), the better the safety of the lithium ion secondary battery, but the battery performance of the lithium ion secondary battery tends to deteriorate. In other words, there is a trade-off between the safety and the battery performance of the lithium ion secondary battery. From this perspective, in order to reduce the resistance of the undercoat layer, the content of the olefin resin (B) is preferably 80% by mass or less, more preferably 75% by mass or less, relative to the total amount of the composition. Furthermore, in order to effectively exhibit the shutdown function, the content of the olefin resin (B) is preferably 35% by mass or more, more preferably 40% by mass or more, even more preferably 50% by mass or more, and particularly preferably 60% by mass or more, relative to the total amount of the composition.
[0039] (1.3) Acrylic Water-Soluble Polymer (C) The composition of the present disclosure contains an acrylic water-soluble polymer (C).
[0040] The content of the acrylic water-soluble polymer (C) is not particularly limited, and is preferably 1% by mass to 20% by mass relative to the total amount of the composition. The content of the acrylic water-soluble polymer (C) is not particularly limited, and is preferably 1% by mass or more, more preferably 2% by mass or more, and even more preferably 3% by mass or more, relative to the total amount of the composition. The content of the acrylic water-soluble polymer (C) is not particularly limited, and is preferably 20% by mass or less, more preferably 15% by mass or less, and even more preferably 10% by mass or less, relative to the total amount of the composition.
[0041] The acrylic water-soluble polymer (C) has structural units derived from (meth)acrylamide and structural units derived from a vinyl monomer having at least one of a carboxy group and a hydroxyl group (hereinafter also referred to as a "specific vinyl monomer"). The content of the structural units derived from (meth)acrylamide is 35% to 95% by mass, based on the total amount of the acrylic water-soluble polymer (C). The content of the structural units derived from the specific vinyl monomer is 5% to 65% by mass, based on the total amount of the acrylic water-soluble polymer (C).
[0042] The glass transition temperature (Tg) of the acrylic water-soluble polymer (C) is not particularly limited, but is preferably 150°C or higher. This results in better heat resistance of the undercoat layer. The glass transition temperature (Tg) of the acrylic water-soluble polymer (C) is not particularly limited, but is preferably 150°C or higher and 400°C or lower. From the viewpoint of obtaining an undercoat layer with better heat resistance, the glass transition temperature (Tg) of the acrylic water-soluble polymer (C) is more preferably 200°C or higher, even more preferably 210°C or higher, particularly preferably 220°C or higher, even more preferably 230°C or higher, and still more preferably 240°C or higher. The glass transition temperature (Tg) of the water-soluble polymer is preferably 400°C or lower, more preferably 300°C or lower, and even more preferably 280°C or lower. The method for measuring the glass transition temperature (Tg) is the same as that described in the examples.
[0043] The content of the (meth)acrylamide-derived structural units is 35% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more, and even more preferably 75% by mass or more, based on the total amount of the acrylic water-soluble polymer (C). From the viewpoint of obtaining an undercoat layer having excellent heat resistance, the content of the (meth)acrylamide-derived structural units is preferably 95% by mass or less, preferably 90% by mass or less, and more preferably 80% by mass or less, based on the total amount of the acrylic water-soluble polymer (C).
[0044] The content of the structural unit derived from the specific vinyl monomer is 5% by mass or more, preferably 10% by mass or more, more preferably 20% by mass or more, based on the total amount of the acrylic water-soluble polymer (C). From the viewpoint of obtaining an undercoat layer having excellent heat resistance, the content of the structural unit derived from the specific vinyl monomer is preferably 65% by mass or less, preferably 40% by mass or less, more preferably 30% by mass or less, based on the total amount of the acrylic water-soluble polymer (C).
[0045] The acrylic water-soluble polymer preferably has a constituent unit derived from (meth)acrylamide, a constituent unit derived from a vinyl monomer having a carboxy group (hereinafter also referred to as a "carboxy group-containing vinyl monomer"), and a constituent unit derived from a vinyl monomer having a hydroxy group (hereinafter also referred to as a "hydroxy group-containing vinyl monomer"), thereby achieving excellent adhesion between the conductive carbon material (A) and the olefin resin (B) and increasing the binding strength due to the interaction between the acrylic polymers.
[0046] When the acrylic water-soluble polymer (C) has a structural unit derived from a carboxy group-containing vinyl monomer and a structural unit derived from a hydroxyl group-containing vinyl monomer, the content of the structural unit derived from the carboxy group-containing vinyl monomer is preferably within the following range. The content of the structural unit derived from the carboxy group-containing vinyl monomer is preferably 3% by mass to 35% by mass, relative to the total amount of the acrylic water-soluble polymer (C). The content of the structural unit derived from the carboxy group-containing vinyl monomer is preferably 3% by mass or more, more preferably 5% by mass or more, and even more preferably 7% by mass or more, relative to the total amount of the acrylic water-soluble polymer (C). From the viewpoint of obtaining an undercoat layer having excellent heat resistance, the content of the structural unit derived from the carboxy group-containing vinyl monomer is preferably 35% by mass or less, more preferably 30% by mass or less, and even more preferably 20% by mass or less, relative to the total amount of the acrylic water-soluble polymer (C).
[0047] When the acrylic water-soluble polymer (C) has a structural unit derived from a carboxy group-containing vinyl monomer and a structural unit derived from a hydroxy group-containing vinyl monomer, the content of the structural unit derived from the hydroxy group-containing vinyl monomer is preferably within the following range. The content of the structural unit derived from the hydroxy group-containing vinyl monomer is preferably 2% by mass to 30% by mass, based on the total amount of the acrylic water-soluble polymer (C). The content of the structural unit derived from the hydroxy group-containing vinyl monomer is preferably 2% by mass or more, more preferably 5% by mass or more, and even more preferably 13% by mass or more, based on the total amount of the acrylic water-soluble polymer (C). From the viewpoint of obtaining an undercoat layer having excellent heat resistance, the content of the structural unit derived from the hydroxy group-containing vinyl monomer is preferably 30% by mass or less, preferably 20% by mass or less, and more preferably 15% by mass or less, based on the total amount of the acrylic water-soluble polymer (C).
[0048] (1.3.1) Raw Material for Acrylic Water-Soluble Polymer (C) The acrylic water-soluble polymer (C) is a polymer obtained by polymerizing an acrylic water-soluble polymer raw material. The raw material for the acrylic water-soluble polymer (C) (hereinafter also referred to as "acrylic water-soluble polymer raw material") contains (meth)acrylamide and a specific vinyl monomer.
[0049] (1.3.1.1) (Meth)acrylamide The (meth)acrylamide may be methacrylamide and acrylamide, or may be methacrylamide or acrylamide. From the viewpoint of improving heat resistance, the (meth)acrylamide is preferably methacrylamide.
[0050] The (meth)acrylamide content is preferably 35% by mass to 95% by mass relative to the total amount of the acrylic water-soluble polymer raw materials. The (meth)acrylamide content is preferably 35% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, and particularly preferably 75% by mass or more, relative to the total amount of the acrylic water-soluble polymer raw materials. From the viewpoint of obtaining excellent heat resistance, the (meth)acrylamide content is preferably 95% by mass or less, preferably 90% by mass or less, and more preferably 80% by mass or less, relative to the total amount of the acrylic water-soluble polymer raw materials.
[0051] (1.3.1.2) Specific Vinyl Monomers Specific vinyl monomers are copolymerizable with (meth)acrylamide and have at least one of a carboxy group and a hydroxyl group.
[0052] The specific vinyl monomer is at least one selected from the group consisting of a carboxyl group-containing vinyl monomer and a hydroxyl group-containing vinyl monomer. From the viewpoints of improving adhesion between the conductive carbon material (A) and the olefin resin (B) and improving adhesion due to interactions between binders, the specific vinyl monomer is preferably a carboxyl group-containing vinyl monomer or a hydroxyl group-containing vinyl monomer.
[0053] The content of the specific vinyl monomer is preferably 5% by mass or more, more preferably 10% by mass or more, and more preferably 20% by mass or more, based on the total amount of the acrylic water-soluble polymer raw material. The content of the specific vinyl monomer is preferably 65% by mass or less, more preferably 40% by mass or less, and even more preferably 30% by mass or less, based on the total amount of the acrylic water-soluble polymer raw material.
[0054] (1.3.1.2.1) Carboxy Group-Containing Vinyl Monomer Examples of the carboxy group-containing vinyl monomer include monocarboxylic acids, dicarboxylic acids, and salts thereof. Examples of the monocarboxylic acid include (meth)acrylic acid. Examples of the dicarboxylic acid include itaconic acid, maleic acid, fumaric acid, itaconic anhydride, maleic anhydride, and fumaric anhydride. These carboxy group-containing vinyl monomers can be used alone or in combination of two or more. The carboxy group-containing vinyl monomer is preferably a monocarboxylic acid, more preferably (meth)acrylic acid, and even more preferably methacrylic acid.
[0055] The content of the carboxy group-containing vinyl monomer is preferably 3% by mass to 35% by mass, relative to the total amount of the acrylic water-soluble polymer raw materials. The content of the carboxy group-containing vinyl monomer is preferably 3% by mass or more, more preferably 5% by mass or more, and more preferably 7% by mass or more, relative to the total amount of the acrylic water-soluble polymer raw materials. The content of the carboxy group-containing vinyl monomer is preferably 35% by mass or less, more preferably 30% by mass or less, and even more preferably 20% by mass or less, relative to the total amount of the acrylic water-soluble polymer raw materials. The content of the carboxy group-containing vinyl monomer is preferably 20% by mass to 95% by mass, relative to the total amount of the specific vinyl monomers. The content of the carboxy group-containing vinyl monomer is preferably 20% by mass or more, more preferably 25% by mass or more, and even more preferably 30% by mass or more, relative to the total amount of the specific vinyl monomers. The content of the carboxy group-containing vinyl monomer is preferably 95% by mass or less, more preferably 90% by mass or less, and even more preferably 85% by mass or less, relative to the total amount of the specific vinyl monomers.
[0056] (1.3.1.2.2) Hydroxyl-containing vinyl monomers Hydroxyl-containing vinyl monomers include vinyl monomers that have a hydroxyl group but no carboxyl group (hereinafter also referred to as "hydroxyl-containing vinyl monomer (c10)") and vinyl monomers that have a hydroxyl group and a carboxyl group (hereinafter also referred to as "hydroxyl-containing vinyl monomer (c20)").
[0057] Examples of the hydroxyl group-containing vinyl monomer (c10) include mono(meth)acrylates (c11) having a hydroxyl group, di(meth)acrylates (c12) having a hydroxyl group, and tri(meth)acrylates (c13) having a hydroxyl group. Examples of the mono(meth)acrylates (c11) having a hydroxyl group include 2-hydroxyethyl(meth)acrylate, 2-hydroxypropyl(meth)acrylate, 3-hydroxypropyl(meth)acrylate, 2-hydroxy-3-phenoxypropyl(meth)acrylate, 3-chloro-2-hydroxypropyl(meth)acrylate, butanediol mono(meth)acrylate, polyethylene glycol mono(meth)acrylate, 2-(6-hydrohexanoyloxy)ethyl acrylate, glycerin mono(meth)acrylate, trimethylolpropane mono(meth)acrylate, and pentaerythritol mono(meth)acrylate. Examples of the di(meth)acrylate (c12) having a hydroxyl group include glycerin di(meth)acrylate, trimethylolpropane di(meth)acrylate, and pentaerythritol di(meth)acrylate. Examples of the tri(meth)acrylate (c13) having a hydroxyl group include pentaerythritol tri(meth)acrylate. These can be used alone or in combination of two or more. The hydroxyl group-containing vinyl monomer (c10) is preferably a mono(meth)acrylate (c11) having a hydroxyl group, and is preferably at least one of 2-hydroxyethyl (meth)acrylate and 2-hydroxypropyl (meth)acrylate, and more preferably 2-hydroxyethyl methacrylate.
[0058] The content of the hydroxyl group-containing vinyl monomer (c10) is preferably 2% by mass to 30% by mass, relative to the total amount of the acrylic water-soluble polymer raw materials. The content of the hydroxyl group-containing vinyl monomer (c10) is preferably 2% by mass or more, more preferably 5% by mass or more, and more preferably 13% by mass or more, relative to the total amount of the acrylic water-soluble polymer raw materials. The content of the hydroxyl group-containing vinyl monomer (c10) is preferably 30% by mass or less, more preferably 20% by mass or less, and even more preferably 15% by mass or less, relative to the total amount of the acrylic water-soluble polymer raw materials. The content of the hydroxyl group-containing vinyl monomer (c10) is preferably 5% by mass to 80% by mass, relative to the total amount of the specific vinyl monomers. The content of the hydroxyl group-containing vinyl monomer (c10) is preferably 5% by mass or more, more preferably 10% by mass or more, and more preferably 15% by mass or more, relative to the total amount of the specific vinyl monomers. The content of the hydroxyl group-containing vinyl monomer (c10) is preferably 80% by mass or less, more preferably 75% by mass or less, and even more preferably 70% by mass or less, based on the total amount of the specific vinyl monomers.
[0059] Examples of the hydroxyl group-containing vinyl monomer (c20) include ricinoleic acid, lesquerolic acid, 15-hydroxylinoleic acid, auricolic acid, hydroxypalmitoleic acid, and caffeic acid. These may be used alone or in combination of two or more.
[0060] (1.3.1.3) Water-soluble copolymerizable monomer The water-soluble acrylic polymer raw material may contain a copolymerizable monomer copolymerizable with (meth)acrylamide and / or a specific vinyl monomer (hereinafter also referred to as a "water-soluble copolymerizable monomer").
[0061] Examples of water-soluble copolymerizable monomers include (meth)acrylic acid alkyl esters (e.g., methyl (meth)acrylate, ethyl (meth)acrylate, etc.), functional group-containing vinyl monomers (e.g., 2-aminoethyl (meth)acrylate, glycidyl (meth)acrylate, (meth)acrylonitrile, allyl sulfonic acid, 2-methacryloyloxyethyl acid phosphate, etc.), vinyl esters (e.g., vinyl acetate, vinyl propionate, etc.), aromatic vinyl monomers (e.g., Examples of the vinyl monomer include vinyl amides (e.g., styrene, α-methylstyrene, etc.), N-substituted unsaturated carboxylic acid amides (e.g., N-methylol(meth)acrylamide, etc.), heterocyclic vinyl compounds (e.g., vinylpyrrolidone, etc.), vinylidene halide compounds (e.g., vinylidene chloride, vinylidene fluoride, etc.), α-olefins (e.g., ethylene, propylene, etc.), dienes (e.g., butadiene, etc.), and crosslinkable vinyl monomers (e.g., methylenebis(meth)acrylamide, divinylbenzene, etc.).
[0062] The content of the water-soluble copolymerizable monomer is within a range in which the water solubility of the water-soluble polymer is maintained, and is, for example, 37% by mass or less, preferably 15% by mass or less, and 0% by mass or more, particularly preferably 0% by mass, relative to the total amount of the acrylic water-soluble polymer raw material.
[0063] (1.3.1.4) Method for Polymerizing Acrylic Water-Soluble Polymer Raw Material A water-soluble polymer can be obtained by polymerizing an acrylic water-soluble polymer raw material using a known method. More specifically, for example, an acrylic water-soluble polymer raw material and a polymerization initiator are mixed with water, the acrylic water-soluble polymer raw material is polymerized, and then, if necessary, aging is performed. There are no particular limitations on the polymerization initiator, and any known polymerization initiator may be used. The polymerization temperature may be 30°C to 95°C. The polymerization time may be 0.5 hours to 20 hours. The aging time may be 0.5 hours to 6 hours.
[0064] (1.4) Additive (D) The composition of the present disclosure may contain an additive (D) as needed. Depending on the type of additive (D), various functions can be imparted to the composition of the present disclosure.
[0065] In the present disclosure, the term "additive" refers to components other than the conductive carbon material (A), the olefin resin (B), and the acrylic water-soluble polymer (C).
[0066] Examples of the additive (D) include a thickening stabilizer, a thermally expandable microcapsule having a maximum volume expansion temperature of 70°C to 180°C (hereinafter simply referred to as "thermally expandable microcapsule"), an inorganic oxide filler, a curable resin filler, a scaly filler, a binder resin, a synthetic rubber, and a non-solid content.
[0067] "Thermally expandable microcapsules" refer to particles having an outer shell made of a thermoplastic resin and a core component, a volatile expanding agent, encapsulated within the outer shell. Specifically, the thermally expandable microcapsules preferably soften, foam, and expand in volume when exposed to temperatures (e.g., 70°C to 160°C) just before the onset of thermal runaway due to abnormal heat generation in a lithium-ion secondary battery while in contact with the electrolyte solution described below. The "maximum volume expansion temperature" refers to the temperature at which the volatile expanding agent encapsulated in the thermally expandable microcapsules gasifies and the thermally expandable microcapsules expand in volume, resulting in a maximum expansion volume. The temperature at which the volatile expanding agent encapsulated in the thermally expandable microcapsules gasifies and the thermally expandable microcapsules begin to expand in volume is referred to as the "volume expansion onset temperature."
[0068] When additive (D) is contained, the content of additive (D) is preferably 1% by mass to 50% by mass relative to the total amount of the composition. When the content of additive (D) is within this range, the shutdown function due to the properties of additive (D) can be more effectively exhibited. The content of additive (D) has little effect on the content ratio of conductive carbon material (A) and olefin resin (B). From the viewpoints of effectively exhibiting the shutdown function and maintaining battery performance, the content of additive (D) is preferably 40% by mass or less, more preferably 30% by mass or less, relative to the total amount of the composition. Furthermore, from the viewpoint of effectively exhibiting the shutdown function, the content of additive (D) is preferably 5% by mass or more, more preferably 10% by mass or more, relative to the total amount of the composition.
[0069] (1.4.1) Thickening stabilizer The composition of the present disclosure may contain a thickening stabilizer. The composition of the present disclosure may not contain a thickening stabilizer. When the composition of the present disclosure contains a thickening stabilizer and is used as a raw material for the undercoat layer, it becomes possible to stably disperse particles when preparing a slurry for the undercoat layer.
[0070] Examples of thickening stabilizers include carboxymethyl cellulose (CMC), polyvinyl alcohol (PVA), methyl cellulose (MC), hydroxypropyl cellulose (HPC), polyethylene glycol (PEG), polyethylene oxide (PEO), polyvinylpyrrolidone (PVP), polyacrylic acid (PAA), polycarboxylic acid ammonium salts, sugars exemplified by glycosides such as lecithin and saponin, and polysaccharides such as xanthan gum, polyether polyols such as sucrose polyether polyol, polyoxypropylene sorbitol ether, trimethylolpropane polyether polyol, and pentaerythritol polyether polyol, oxidized starch, starch phosphate, casein, and various modified starches.
[0071] The content of the thickening stabilizer is preferably 1% by mass to 50% by mass relative to the total amount of the composition. From the viewpoint of effectively exhibiting the shutdown function and maintaining battery performance, the content of the thickening stabilizer is preferably 15% by mass or less, more preferably 10% by mass or less, relative to the total amount of the composition. From the viewpoint of more effectively dispersing the fine particles in the undercoat slurry, the content of the thickening stabilizer is preferably 1% by mass or more, more preferably 2% by mass or more, relative to the total amount of the composition.
[0072] Commercially available CMC products include "1130", "1140", "1240", "1250", "1260", "1330", "2200", and "DL100L" manufactured by Daicel Miraize Co., Ltd.
[0073] (1.4.2) Thermally Expandable Microcapsules The composition of the present disclosure may contain thermally expandable microcapsules. The composition of the present disclosure may not contain thermally expandable microcapsules. When the composition of the present disclosure contains thermally expandable microcapsules and is used as a raw material for the undercoat layer, the thermally expandable microcapsules undergo volumetric expansion due to abnormal heat generation in the lithium ion secondary battery, efficiently increasing the DC resistance of the electrode and improving the safety of the lithium ion secondary battery.
[0074] The volume expansion starting temperature of the thermally expandable microcapsules is preferably 100° C. to 180° C., more preferably 110° C. to 150° C., and even more preferably 120° C. to 130° C. The maximum volume expansion temperature of the thermally expandable microcapsules is preferably 100° C. to 180° C., more preferably 120° C. to 170° C., and even more preferably 145° C. to 155° C.
[0075] The thermoplastic resin constituting the outer shell preferably contains a (co)polymer containing vinylidene chloride and a (co)polymer containing (meth)acrylonitrile. This allows the thermoplastic resin constituting the outer shell to have excellent electrolyte resistance, thermoplasticity, and gas barrier properties. From the viewpoint of electrolyte resistance, the thermoplastic resin constituting the outer shell is preferably a (co)polymer containing (meth)acrylonitrile as the main component (51% by mass or more). The raw material for the thermoplastic resin constituting the outer shell may contain a crosslinkable monomer in addition to a polymerizable monomer in order to improve the foaming properties and heat resistance of the resulting thermally expandable microcapsules.
[0076] The boiling point of the volatile expanding agent is preferably selected so that the maximum volume expansion temperature of the thermally expandable microcapsules is higher than the softening point of the olefin-based resin (B). The boiling point is preferably selected so that the volume expansion initiation temperature of the thermally expandable microcapsules is equal to the softening point of the olefin-based resin (B). This effectively increases the DC resistance of the electrode when the temperature of the undercoat layer rises above the softening point of the olefin-based resin (B) due to heat generation in the lithium-ion secondary battery. As a result, the safety of the lithium-ion secondary battery is further improved. Examples of volatile expanding agents include low-molecular-weight hydrocarbons with a boiling point of 100°C or less, non-flammable or flame-retardant compounds, and the like. Low-molecular-weight hydrocarbons are preferably used as low-molecular-weight hydrocarbons with a boiling point of 100°C or less. Examples of low-molecular-weight hydrocarbons include propane, propylene, n-butane, isobutane, butene, isobutene, isopentane, neopentane, n-pentane, n-hexane, isohexane, heptane, and petroleum ether. Examples of non-flammable or flame-retardant compounds include halogenated hydrocarbons (e.g., methyl chloride, methylene chloride, fluorotrichloromethane, difluorodichloromethane, chlorotrifluoromethane, etc.), chlorofluorocarbons, etc. The volatile expanding agents may be used alone or in combination of two or more.
[0077] The particle size of the thermally expandable microcapsules is not particularly limited, but is preferably 1 μm to 40 μm, more preferably 3 μm to 30 μm, and even more preferably 5 μm to 25 μm.
[0078] The particle size of the thermally expandable microcapsules is the particle size (particle size distribution D50, median diameter) corresponding to a cumulative 50 volume % from the fine particle side in the volume-based particle size distribution measured using a particle size distribution measuring device based on the laser light diffraction scattering method.
[0079] The content of the thermally expandable microcapsules is preferably 0% by mass to 50% by mass relative to the total amount of the composition. The content of the thermally expandable microcapsules has little effect on the content ratio of the conductive carbon material (A) and the olefin-based resin (B), and from the viewpoints of maintaining the shutdown function and battery performance, the content is preferably 50% by mass or less, more preferably 40% by mass or less, relative to the total amount of the composition. Furthermore, from the viewpoint of enhancing the shutdown function due to the thermal expansion of the thermally expandable microcapsules in the event of abnormal heat generation, the content of the thermally expandable microcapsules is preferably 5% by mass or more, more preferably 10% by mass or more, relative to the total amount of the composition.
[0080] The thermally expandable microcapsules may be commercially available products, such as the Matsumoto Microsphere (registered trademark) series manufactured by Matsumoto Yushi Seiyaku Co., Ltd., the EXPANCEL (registered trademark) series manufactured by Akzo Nobel, or the ADVANCEL (registered trademark) series manufactured by Sekisui Chemical Co., Ltd.
[0081] (1.4.3) Inorganic Oxide Filler The composition of the present disclosure may contain an inorganic oxide filler. The composition of the present disclosure may not contain an inorganic oxide filler. When the composition of the present disclosure contains an inorganic oxide filler, the inorganic oxide filler functions as a filler. Increasing the content of the inorganic oxide filler contributes to improving the heat resistance of the positive electrode, while minimizing the content of the inorganic oxide filler forms an undercoat layer that adheres to the positive electrode mixture layer. In the event of an internal short circuit, the undercoat layer melts, contributing to improved safety. Furthermore, by selecting the type and physical properties of the inorganic oxide filler, it is possible to decompose the electrolyte and generate gas when the battery is overcharged.
[0082] The inorganic oxide filler may be aluminum oxide (α-Al 2 O 3 , γ-Al 2 O 3 ), aluminum hydroxide (Al(OH) 3 ), boehmite (AlOOH), magnesia (magnesium oxide: MgO), magnesium hydroxide (Mg(OH)2 ), zirconia (ZrO 2 ), titania (TiO 2 ), silica (SiO 2 ), silicon dioxide (SiO 2 ), silicon carbide (SiC), aluminum nitride (AlN), boron nitride (BN), mica, or graphite oxide (e.g., expanded graphite). The inorganic oxide filler may be used alone or in combination of two or more. Among these, the inorganic oxide filler preferably contains aluminum oxide.
[0083] The shape of the inorganic oxide filler is not particularly limited, and examples thereof include spherical, needle-like, ellipsoidal, plate-like, and scale-like shapes. The particle size of the inorganic oxide filler is not particularly limited, and is preferably 0.01 μm to 5 μm. The particle size of the inorganic oxide filler indicates a particle size (particle size distribution D50, median diameter) corresponding to a cumulative 50% by volume from the fine particle side in a volume-based particle size distribution measured using a particle size distribution measuring device based on a laser light diffraction scattering method.
[0084] The content of the inorganic oxide filler is preferably 0% by mass to 50% by mass relative to the total amount of the composition. The content of the inorganic oxide filler has little effect on the content ratio of the conductive carbon material (A) and the olefin-based resin (B), and from the viewpoints of maintaining the shutdown function and battery performance, the content is preferably 40% by mass or less, more preferably 30% by mass or less, relative to the total amount of the composition. Furthermore, the content of the inorganic oxide filler is preferably 5% by mass or more, more preferably 10% by mass or more, relative to the total amount of the composition, from the viewpoints of suppressing the fluidity of the olefin-based resin (B) dissolved in the undercoat layer at high temperatures and maintaining the shutdown function for a long period of time.
[0085] (1.4.4) Binder Resin The composition of the present disclosure may contain a binder resin as another component. When the composition of the present disclosure is used as a raw material for an undercoat layer, the binder resin can improve the physical properties of the undercoat layer (e.g., electrolyte permeability and peel strength) and also improve the battery performance of the lithium-ion secondary battery.
[0086] Examples of binder resins include polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), PVDF copolymers, hydroxypropyl methylcellulose, polyvinyl alcohol, and diacetyl cellulose. PVDF copolymers are copolymers of vinylidene fluoride and other monomers, such as PVDF-HFP (hexafluoropropylene) and PVDF-PEO (polyoxyethylene). Of these, it is preferable that the binder resin contain PVDF from the viewpoint of reducing the resistance of the undercoat layer.
[0087] As the binder resin, commercially available products on the market may be used. Commercially available PVDF products include the KUREHA (registered trademark) KF Polymer series manufactured by KUREHA CORPORATION, such as "W#1100", "W#1300", "W#1700", "W#7200", and "W#7300".
[0088] The binder resin may be used alone or in combination of two or more. The content of the binder resin is preferably 1% by mass to 20% by mass relative to the total amount of the composition. The shutdown function depends on the balance between the content of the binder resin and the total content of the olefin resin (B) and the acrylic water-soluble polymer (C). When the content ratio of the binder resin to the total amount of the composition is high, the content ratio of the olefin resin (B) and the acrylic water-soluble polymer (C) to the total amount of the composition becomes low, which may result in a decrease in the shutdown function. When the content of the binder resin is within the above range, it is possible to achieve both processability of the composition (e.g., slurry for the undercoat layer) and ensuring the shutdown function. The content of the binder resin is preferably 15% by mass or less, more preferably 10% by mass or less, relative to the total amount of the composition, from the viewpoint of ensuring the shutdown function in relation to the content of the olefin resin (B) and the acrylic water-soluble polymer (C). From the viewpoint of processability of the composition (for example, slurry for the undercoat layer), the content of the binder resin is preferably 2% by mass or more, and more preferably 3% by mass or more, relative to the total amount of the composition.
[0089] (1.4.5) Synthetic Rubber The composition of the present disclosure may contain a synthetic rubber as another component. When the composition of the present disclosure is used as a raw material for an undercoat layer, this improves the adhesion between the undercoat layer and the current collector, thereby enabling a further reduction in battery resistance.
[0090] Examples of synthetic rubbers include styrene butadiene rubber (SBR), acrylonitrile-butadiene rubber, acrylonitrile-butadiene-styrene rubber, hydrogenated styrene butadiene rubber (HSBR), butylene rubber, polybutadiene, and polyisoprene rubber. Among these, from the viewpoint of low resistance of the undercoat layer, synthetic rubbers appropriately mixed with a water-dispersible binder such as an emulsion of SBR are preferred, and it is more preferred that the synthetic rubber contains SBR. The synthetic rubbers may be used alone or in combination of two or more.
[0091] The shape of the synthetic rubber is not particularly limited, and it may be in the form of particles.
[0092] As the synthetic rubber, commercially available products may be used, such as "TRD2001" (aqueous dispersion of styrene butadiene rubber particles) manufactured by JSR Corporation.
[0093] (1.4.6) Non-Solid Content The composition of the present disclosure may contain non-solid content, such as various formulation components derived from the undercoat layer slurry (e.g., surfactants, dispersants, wetting agents, antifoaming agents, etc.), water, etc.
[0094] The composition of the present disclosure further contains an additive (D), and the content of the additive (D) is preferably 1 mass % to 50 mass % relative to the total amount of the composition, and the additive (D) preferably contains carboxymethyl cellulose, which can stabilize the dispersion of the fine particles in the undercoat slurry.
[0095] The composition of the present disclosure further contains an additive (D), and the content of the additive (D) is preferably 1% by mass to 50% by mass relative to the total amount of the composition, and the additive (D) preferably includes at least one of thermally expandable microcapsules and an inorganic oxide filler having a maximum volume expansion temperature of 70° C. to 180° C. This makes it easier for the olefin-based resin (B) to exhibit its shutdown function.
[0096] The composition of the present disclosure further contains an additive (D), and the content of the additive (D) is preferably 1% by mass to 50% by mass relative to the total amount of the composition, and the additive (D) preferably contains aluminum oxide, which makes it easier for the olefin-based resin (B) to exhibit its shutdown function.
[0097] (1.5) Physical Properties of the Composition Various physical properties of the composition of the present disclosure will be described.
[0098] In the composition of the present disclosure, from the viewpoint of forming an electrode that is excellent in safety, has low DC resistance during initial charge / discharge, and is suppressed from increasing in DC resistance in a high-temperature environment, the ratio of particle size distribution D99 to particle size distribution D10 (D99 / D10), measured by a laser light diffraction / scattering method, is preferably 35 or less.
[0099] "Particle size distribution D99 measured by laser light diffraction scattering" refers to the particle size corresponding to the cumulative 99% by volume from the fine particle side in the volume-based particle size distribution measured by a particle size distribution measuring device based on laser light diffraction scattering. The method for measuring D99 is the same as that described in the Examples. "Particle size distribution D10 measured by laser light diffraction scattering" refers to the particle size corresponding to the cumulative 10% by volume from the fine particle side in the volume-based particle size distribution measured by a particle size distribution measuring device based on laser light diffraction scattering. The method for measuring D10 is the same as that described in the Examples.
[0100] A ratio (D99 / D10) of 35 or less indicates a small number of aggregates of components in the composition (in other words, a large number of components dispersed in the composition). That is, the lower the ratio (D99 / D10), the fewer the number of aggregates of components in the composition. The conductive carbon material (A) in the composition is uniformly dispersed, facilitating the formation of a uniform conductive path within the undercoat layer. This suppresses the initial DC resistance during battery charge / discharge and the increase in DC resistance after long-term storage in a high-temperature environment. Furthermore, the uniform dispersion of the olefin resin (B) and the acrylic water-soluble polymer (C) in the composition facilitates efficient shutdown function. As a result, the composition of the present disclosure is highly safe and enables the formation of an electrode that exhibits low DC resistance during initial charge / discharge and significantly suppresses the increase in DC resistance in a high-temperature environment. Therefore, a lithium-ion secondary battery with excellent battery performance can be obtained.
[0101] From the viewpoint of improving the safety and battery performance of the lithium ion secondary battery, the ratio (D99 / D10) is more preferably 3.0 to 30.0, even more preferably 3.0 to 22.0, and particularly preferably 3.0 to 15.0.
[0102] Methods for adjusting the ratio (D99 / D10) within the above range include a kneader, a two-roll mill, a three-roll mill, a planetary mixer, a ball mill, a horizontal sand mill, a vertical sand mill, an annular bead mill, an attritor, a high-shear mixer, a Disper, a Filmix, an ultrasonic or high-pressure homogenizer, and the like.
[0103] In the composition of the present disclosure, the particle size distribution D99 measured by laser light diffraction scattering is preferably 20 μm or less. The smaller the aggregates of fine particles, the better the dispersibility of the materials contained in the composition. A D99 of 20 μm or less makes it easier to improve the safety and battery performance of lithium ion secondary batteries compared to when D99 exceeds 20 μm. From the viewpoint of improving the safety and battery performance of lithium ion secondary batteries, the D99 of the composition is more preferably 2.0 μm to 20.0 μm, even more preferably 2.0 μm to 15.0 μm, and particularly preferably 2.0 μm to 10.0 μm.
[0104] Methods for adjusting the D99 of the composition to fall within the above range include a kneader, a two-roll mill, a three-roll mill, a planetary mixer, a ball mill, a horizontal sand mill, a vertical sand mill, an annular bead mill, an attritor, a high-shear mixer, a Disper, a Filmix, an ultrasonic or high-pressure homogenizer, and the like.
[0105] The particle size distribution D10 of the composition of the present disclosure, as measured by a laser light diffraction scattering method, is preferably 0.1 μm to 1.5 μm, more preferably 0.1 μm to 1.0 μm, and even more preferably 0.1 μm to 0.7 μm. From the viewpoint of dispersibility, the particle size distribution D10 is preferably 0.2 μm to 1.0 μm, and more preferably 0.4 μm to 1.0 μm. When D10 is within the above range, the dispersibility of the materials contained in the composition is excellent, and the safety and battery performance of the lithium ion secondary battery are more likely to be improved than when D10 is not within the above range.
[0106] Methods for adjusting D10 to within the above range include a kneader, a two-roll mill, a three-roll mill, a planetary mixer, a ball mill, a horizontal sand mill, a vertical sand mill, an annular bead mill, an attritor, a high-shear mixer, a Disper, a Filmix, an ultrasonic or high-pressure homogenizer, and the like.
[0107] In the composition of the present disclosure, the ratio (D99 / D50) of particle size distribution D99 to particle size distribution D50 (also simply referred to as "D50") measured by laser light diffraction scattering is preferably 20 or less. A ratio (D99 / D50) of 20 or less indicates that the size of aggregates is suppressed relative to the median diameter of fine particles in the composition. A ratio (D99 / D50) of 20 or less results in excellent dispersibility of the composition. This makes it easier to improve the safety and battery performance of lithium ion secondary batteries compared to when the ratio (D99 / D50) exceeds 20. From the viewpoint of improving the safety and battery performance of lithium ion secondary batteries, the ratio (D99 / D50) is more preferably 2.0 to 16.0, even more preferably 2.0 to 10.0, and particularly preferably 2.0 to 6.0.
[0108] "Particle size distribution D50 measured by laser light diffraction scattering" refers to the particle size corresponding to 50% by volume cumulative from the fine particle side in the volume-based particle size distribution measured by a particle size distribution measuring device based on laser light diffraction scattering. The method for measuring D50 is the same as that described in the Examples.
[0109] Methods for adjusting the ratio (D99 / D50) within the above range include a kneader, a two-roll mill, a three-roll mill, a planetary mixer, a ball mill, a horizontal sand mill, a vertical sand mill, an annular bead mill, an attritor, a high-shear mixer, a Disper, a Filmix, an ultrasonic or high-pressure homogenizer, and the like.
[0110] The particle size distribution D50 of the composition of the present disclosure, as measured by a laser light diffraction scattering method, is not particularly limited and is preferably 0.5 μm to 5.0 μm, more preferably 0.5 μm to 3.0 μm, and even more preferably 0.5 μm to 2.0 μm. If the D50 is within the above range, the dispersibility of the composition is excellent, and the safety and battery performance of the lithium ion secondary battery are likely to be improved.
[0111] Methods for adjusting D50 within the above range include a kneader, a two-roll mill, a three-roll mill, a planetary mixer, a ball mill, a horizontal sand mill, a vertical sand mill, an annular bead mill, an attritor, a high-shear mixer, a Disper, a Filmix, an ultrasonic or high-pressure homogenizer, and the like.
[0112] The particle size distribution D90 (also simply referred to as "D90") of the composition of the present disclosure measured by a laser light diffraction scattering method is preferably 1.0 μm to 10.0 μm, more preferably 1.0 μm to 7.0 μm, and even more preferably 1.0 μm to 4.0 μm. When D90 is within the above range, the dispersibility of the composition is excellent, and it is easy to improve the safety and battery performance of lithium ion secondary batteries. "Particle size distribution D90 measured by a laser light diffraction scattering method" refers to the particle size corresponding to the cumulative 90% by volume from the fine particle side in a volume-based particle size distribution measured using a particle size distribution measuring device based on the laser light diffraction scattering method. The method for measuring D90 is the same as that described in the Examples.
[0113] Methods for adjusting D90 within the above range include a kneader, a two-roll mill, a three-roll mill, a planetary mixer, a ball mill, a horizontal sand mill, a vertical sand mill, an annular bead mill, an attritor, a high-shear mixer, a Disper, a Filmix, an ultrasonic or high-pressure homogenizer, and the like.
[0114] (1.6) Preferred Composition With regard to the content ratios of the above-mentioned conductive carbon material (A), olefin resin (B), and acrylic water-soluble polymer (C), from the viewpoint of effectively exhibiting the shutdown function and maintaining battery performance, it is preferred that the content of the conductive carbon material (A) is 1% by mass to 30% by mass relative to the total amount of the composition, the content of the olefin resin (B) is 30% by mass to 90% by mass relative to the total amount of the composition, and the content of the acrylic water-soluble polymer (C) is 1% by mass to 20% by mass relative to the total amount of the composition.
[0115] (1.6.1) Preferred Composition (i) In addition to the configuration described above, the composition of the present disclosure preferably satisfies the following requirement (a1). This allows for excellent adhesion between the conductive carbon material (A) and the olefin resin (B), and battery performance can be maintained. In addition to the configuration described above, the composition of the present disclosure preferably satisfies the following requirements (a1) and (a2). This improves the balance between effective exertion of the shutdown function and maintenance of battery performance. In addition to the configuration described above, the composition of the present disclosure preferably satisfies the following requirements (a1), (a2), and (a3). This improves the balance between effective exertion of the shutdown function and maintenance of battery performance. In addition to the configuration described above, the composition of the present disclosure preferably satisfies the following requirements (a1), (a2), (a3), and (a4). This allows the energy density of the lithium secondary battery to be maintained, and improves the balance between effective exertion of the shutdown function and maintenance of battery performance. In addition to the configuration described above, the composition of the present disclosure preferably satisfies the following requirements (a1), (a2), (a3), (a4), and (a5). This results in excellent high-temperature treatment resistance of the electrode, allows the energy density of the lithium secondary battery to be maintained, and improves the balance between effective exertion of the shutdown function and maintenance of battery performance. In addition to the above-mentioned configuration, the composition of the present disclosure preferably satisfies the following requirements (a1), (a2), (a3), (a4), (a5), and (a6). As a result, when the composition of the present disclosure is applied to a lithium secondary battery equipped with an electrode, a lithium ion secondary battery with a better balance between safety and battery performance (i.e., output and life) can be obtained.
[0116] (1.6.1.1) Requirements (a1) to (a6) Requirement (a1): The content of structural units derived from (meth)acrylamide is 60% to 85% by mass relative to the total amount of the acrylic water-soluble polymer (C). Requirement (a2): The content of the conductive carbon material (A) is 10% to 20% by mass relative to the total amount of the composition. Requirement (a3): The content of the olefin resin (B) is 60% to 80% by mass relative to the total amount of the composition. Requirement (a4): The particle size of the olefin resin (B) is 1 μm to 3 μm. Requirement (a5): The softening point of the olefin resin (B) is 120° C. or higher. Requirement (a6): The composition of the present disclosure further contains an additive (D), and the additive (D) includes CMC.
[0117] (1.6.2) Preferred Composition (ii) In addition to the configuration described above, the composition of the present disclosure preferably satisfies the following requirement (b1). This allows for excellent adhesion between the conductive carbon material (A) and the olefin resin (B), and battery performance can be maintained. In addition to the configuration described above, the composition of the present disclosure preferably satisfies the following requirements (b1) and (b2). This improves the balance between effective exertion of the shutdown function and maintenance of battery performance. In addition to the configuration described above, the composition of the present disclosure preferably satisfies the following requirements (b1), (b2), and (b3). This improves the balance between effective exertion of the shutdown function and maintenance of battery performance. In addition to the configuration described above, the composition of the present disclosure preferably satisfies the following requirements (b1), (b2), (b3), and (b4). This allows the energy density of the lithium secondary battery to be maintained, and improves the balance between effective exertion of the shutdown function and maintenance of battery performance. In addition to the configuration described above, the composition of the present disclosure preferably satisfies the following requirements (b1), (b2), (b3), (b4), and (b5). This results in excellent high-temperature treatment resistance of the electrode, allows the energy density of the lithium secondary battery to be maintained, and improves the balance between effective exertion of the shutdown function and maintenance of battery performance. In addition to the above-mentioned configuration, the composition of the present disclosure preferably satisfies the following requirements (b1), (b2), (b3), (b4), (b5), and (b6). As a result, when the composition of the present disclosure is applied to a lithium secondary battery equipped with an electrode, it is possible to obtain a lithium ion secondary battery having an especially excellent balance between safety and battery performance (i.e., output and life).
[0118] (1.6.2.1) Requirements (b1) to (b6) Requirement (b1): The content of the structural unit derived from (meth)acrylamide is 60% by mass to 85% by mass relative to the total amount of the acrylic water-soluble polymer (C). Requirement (b2): The content of the conductive carbon material (A) is 10% by mass to 20% by mass relative to the total amount of the composition. Requirement (b3): The content of the olefin resin (B) is 70% by mass to 80% by mass relative to the total amount of the composition. Requirement (b4): The particle size of the olefin resin (B) is 1 μm to 2 μm. Requirement (b5): The softening point of the olefin resin (B) is 120° C. or higher. Requirement (b6): The composition of the present disclosure further contains an additive (D), and the additive (D) includes CMC.
[0119] (1.7) Method for Producing Composition The method for producing a composition according to the present disclosure preferably includes the steps of mixing the conductive carbon material (A), the olefin resin (B), and the acrylic water-soluble polymer (C) to prepare a mixture (hereinafter also referred to as the "mixing step"), and dispersing the mixture using a dispersing roll (hereinafter also referred to as the "dispersing step"). The mixing step and the dispersing step can be carried out in this order, and when carried out in this order, another step (for example, a step of kneading the mixture) may be included between the mixing step and the dispersing step.
[0120] (1.7.1) Mixing Step In the mixing step, the conductive carbon material (A), the olefin resin (B), and the acrylic water-soluble polymer (C) are mixed to prepare a mixture. The mixing method is not particularly limited, and any known method may be used. The blending amounts of the conductive carbon material (A), the olefin resin (B), and the acrylic water-soluble polymer (C) are the same as the ranges described above for the contents of the conductive carbon material (A), the olefin resin (B), and the acrylic water-soluble polymer (C) in the composition of the present disclosure.
[0121] (1.7.2) Dispersion Step In the dispersion step, the mixture is dispersed using a dispersion roll. This results in a composition in which the raw materials are more dispersed than in the mixture before the dispersion step. As a result, when the prepared electrode is installed in a secondary battery, the obtained composition not only reduces the DC resistance during initial charge and discharge, but also effectively suppresses the increase in DC resistance in a high-temperature environment compared to when the dispersion step is not performed. The process of dispersing the mixture using a dispersion roll is also called the "dispersion treatment." The mixture may be kneaded in advance before the dispersion treatment.
[0122] The dispersion method is not particularly limited, and examples include methods using a kneading device. Examples of kneading devices include kneaders, two-roll mills, three-roll mills, planetary mixers, ball mills, horizontal sand mills, vertical sand mills, annular bead mills, attritors, high-shear mixers, Dispersers, Filmix, ultrasonic or high-pressure homogenizers, etc. Among these, a three-roll mill is preferred as the kneading device from the viewpoint of more uniformly dispersing the fine particles in the mixture. When a kneading device is used, examples of the dispersion method for the mixture include batch dispersion, pass dispersion, and circulation dispersion. Two or more methods may be combined to disperse the mixture. "Batch dispersion" refers to a method in which the mixture is dispersed using only a kneading device without using piping, etc. "Pass dispersion" refers to a method in which the mixture is dispersed by passing the mixture through the kneading device using a kneading system. The kneading system includes a kneading device, a first tank that supplies the mixture to the kneading device via piping, and a second tank that receives the mixture after the kneading process. "Circulation dispersion" refers to a method in which the mixture after the kneading treatment in the second tank is returned to the first tank and dispersed while being circulated.
[0123] The three-roll mill will be described with reference to Fig. 4. In Fig. 4, the symbol D1 indicates the rotation direction of the first roll 91 (hereinafter also referred to as the "feed roll 91"). The symbol D2 indicates the rotation direction of the second roll 92 (hereinafter also referred to as the "intermediate roll 92"). The symbol D3 indicates the rotation direction of the third roll 93 (hereinafter also referred to as the "finishing roll 93").
[0124] As shown in Figure 4, the three-roll mill 90 includes a feed roll 91, an intermediate roll 92, a finishing roll 93, and a blade 94. The feed roll 91 and the intermediate roll 92 are disposed with a first distance L1 (see Figure 4) between them. The intermediate roll 92 and the finishing roll 93 are disposed with a second distance L2 (see Figure 4) between them. The blade 94 is disposed so as to come into contact with the surface of the finishing roll 93.
[0125] In the three-roll mill 90, as shown in Fig. 4, a mixture 1110 is stored in an upper space formed by a feed roll 91 and an intermediate roll 92. The mixture 1110 adhering to the surface of the feed roll 91 is transferred to the surface of the intermediate roll 92. The mixture 1110 adhering to the surface of the intermediate roll 92 is transferred to the surface of the finishing roll 93. The mixture 1110 adhering to the surface of the finishing roll 93 is scraped off by a blade 94.
[0126] The feed roll 91, the intermediate roll 92, and the finishing roll 93 may each be a roll used in a known three-roll mill. The feed roll 91, the intermediate roll 92, and the finishing roll 93 each have approximately the same diameter. The blade 94 may be, for example, a doctor blade.
[0127] The rotation speeds of the feed roll 91, the intermediate roll 92, and the finishing roll 93 are not particularly limited, and may be faster in the order of the feed roll 91, the intermediate roll 92, and the finishing roll 93. The rotation speed of the feed roll 91 is not particularly limited, and is preferably 5 revolutions per minute (rpm) to 84 rpm, and more preferably 16 rpm to 56 rpm. The rotation speed of the intermediate roll 92 is not particularly limited, and is preferably 16 rpm to 240 rpm, and more preferably 50 rpm to 160 rpm. The rotation speed of the finishing roll 93 is not particularly limited, and is preferably 50 rpm to 600 rpm, and more preferably 150 rpm to 400 rpm. The ratio of the rotational speed of the intermediate roll 92 to the rotational speed of the feed roll 91 (rotational speed of the intermediate roll 92 / rotational speed of the feed roll 91) is preferably 2.0 to 4.0, more preferably 2.5 to 3.5, from the viewpoint of uniformly dispersing the fine particles in the mixture. The ratio of the rotational speed of the finishing roll 93 to the rotational speed of the feed roll 91 (rotational speed of the finishing roll 93 / rotational speed of the feed roll 91) is preferably 5.0 to 12.0, more preferably 6.5 to 10.0, from the viewpoint of uniformly dispersing the fine particles in the mixture.
[0128] The first distance L1 is not particularly limited, and from the viewpoint of uniformly dispersing the fine particles in the mixture, it is preferably 0 mm to 0.05 mm, more preferably 0 mm to 0.02 mm. The second distance L2 is not particularly limited, and from the viewpoint of uniformly dispersing the fine particles in the mixture, it is preferably 0 mm to 0.05 mm, more preferably 0 mm to 0.02 mm.
[0129] The number of dispersion treatments (hereinafter also referred to as "number of treatments") may be one or more. Among these, the number of treatments is preferably three. When the number of treatments is three, the conductive carbon material (A) and the olefin-based resin (B) in the mixture are more likely to be uniformly dispersed than when the number of treatments is two or less or four or more. As a result, a composition is obtained that can be used to form a lithium ion secondary battery in which the DC resistance at the initial stage of charge / discharge and the increase in DC resistance under high-temperature environments (particularly after long-term storage) are more effectively suppressed.
[0130] (2) Undercoat The undercoat layer of the present disclosure contains the composition of the present disclosure as described above. The composition of the present disclosure is as described above, so further description will be omitted here.
[0131] The thickness of the undercoat layer is not particularly limited. The thickness of the undercoat layer is preferably 50 μm or less, more preferably 20 μm or less, from the viewpoint of further suppressing the DC resistance of the lithium ion secondary battery during normal operation. The thickness of the undercoat layer is preferably 0.1 μm or more, more preferably 0.2 μm or more, from the viewpoint of further increasing the DC resistance during abnormal heat generation of the lithium ion secondary battery and more reliably exhibiting the shutdown function.
[0132] The position where the undercoat layer is formed is preferably at least a part of at least one main surface of the positive electrode current collector, and may be appropriately selected depending on the coating pattern of the positive electrode mixture layer (for example, intermittent coating, stripe coating, etc.).
[0133] (3) Electrode The electrode of the present disclosure includes a current collector, the undercoat layer of the present disclosure, and a composite layer. The "electrode" refers to at least one of the positive electrode and the negative electrode of a lithium ion secondary battery.
[0134] The electrode of the present disclosure has the above-described configuration, and therefore can be used to fabricate a lithium ion secondary battery that is excellent in safety and in which an increase in DC resistance is suppressed during the initial charge / discharge cycle and in high-temperature environments (especially after long-term storage).
[0135] The electrode of the present disclosure preferably has a current collector, an undercoat layer, and a composite layer laminated in this order. As a result, the electrode of the present disclosure increases the electrical resistance between the current collector and the composite layer when the temperature of the lithium-ion secondary battery rises suddenly. This prevents the lithium-ion secondary battery from overheating. Therefore, the electrode of the present disclosure can improve the safety of the lithium-ion secondary battery. Furthermore, the electrode of the present disclosure can prevent an increase in DC resistance in the lithium-ion secondary battery even when the lithium-ion secondary battery is stored in a high-temperature environment for a long period of time.
[0136] The electrode of the present disclosure may be a positive electrode or a negative electrode. In particular, the electrode of the present disclosure is preferably a positive electrode. When the electrode of the present disclosure is a positive electrode, the electrical resistance of the positive electrode increases, thereby allowing the resulting lithium ion secondary battery to exhibit a good shutdown function.
[0137] (3.1) Positive Electrode The positive electrode of the present disclosure may include a current collector (hereinafter also referred to as a "positive electrode current collector"), an undercoat layer, and a composite layer (hereinafter also referred to as a "positive electrode composite layer").
[0138] The positive electrode of the present disclosure includes a first positive electrode configuration, a second positive electrode configuration, a third positive electrode configuration, and a fourth positive electrode configuration. The first positive electrode configuration indicates a configuration in which an undercoat layer and a positive electrode composite layer are laminated in this order on both main surfaces of a current collector. The second positive electrode configuration indicates a configuration in which an undercoat layer and a positive electrode composite layer are laminated in this order on one main surface of a current collector, and an undercoat layer is laminated on the other main surface of the current collector. The third positive electrode configuration indicates a configuration in which an undercoat layer and a positive electrode composite layer are laminated in this order on one main surface of a current collector, and a positive electrode composite layer is laminated on the other main surface of the current collector. The fourth positive electrode configuration indicates a configuration in which an undercoat layer and a positive electrode composite layer are laminated in this order on one main surface of a current collector, and neither the undercoat layer nor the positive electrode composite layer is laminated on the other main surface of the current collector.
[0139] (3.1.1) Positive Electrode Current Collector Examples of the material for the positive electrode current collector include aluminum, nickel, stainless steel (SUS), copper, etc. "Aluminum" includes pure aluminum and aluminum alloys.
[0140] (3.1.2) Undercoat Layer Details of the undercoat layer and the composition forming it have been described above, and therefore further description will be omitted here.
[0141] (3.1.3) Positive Electrode Mixture Layer The positive electrode mixture layer contains a positive electrode active material and a binder.
[0142] (3.1.3.1) Positive Electrode Active Material The positive electrode active material is not particularly limited as long as it is a material that can absorb and release lithium ions, and can be adjusted appropriately depending on the application of the lithium ion secondary battery.
[0143] Examples of positive electrode active materials include a first oxide and a second oxide. The first oxide contains lithium (Li) and nickel (Ni) as constituent metal elements. The second oxide contains Li, Ni, and at least one metal element other than Li and Ni as constituent metal elements. Examples of metal elements other than Li and Ni include transition metal elements and typical metal elements. The second oxide preferably contains the metal elements other than Li and Ni in an amount equivalent to or less than Ni in atomic number terms. The metal elements other than Li and Ni may be, for example, at least one selected from the group consisting of Co, Mn, Al, Cr, Fe, V, Mg, Ca, Na, Ti, Zr, Nb, Mo, W, Cu, Zn, Ga, In, Sn, La, and Ce. The positive electrode active materials may be used alone or in combination of two or more.
[0144] The positive electrode active material preferably contains a lithium-containing composite oxide (hereinafter, sometimes referred to as "NCM") represented by the following formula (X): The lithium-containing composite oxide (X) has the advantages of high energy density per unit volume and excellent thermal stability.
[0145] LiNi a Co b Mn c O 2 ... Formula (X)
[0146] In formula (X), a, b, and c each independently represent a number greater than 0 and less than 1, and the sum of a, b, and c is 0.99 to 1.00.
[0147] Specific examples of NCM include LiNi 0.33 Co 0.33 Mn 0.33 O 2 , LiNi 0.5 Co 0.3 Mn 0.2 O 2 , LiNi 0.5 Co 0.2 Mn 0.3 O 2 , LiNi 0.6 Co 0.2 Mn 0.2 O2 , LiNi 0.8 Co 0.1 Mn 0.1 O 2 Examples include:
[0148] The positive electrode active material may contain a lithium-containing composite oxide (hereinafter, sometimes referred to as "NCA") represented by the following formula (Y).
[0149] Li t Ni 1-x-y Co x Al y O 2 ... Formula (Y)
[0150] In formula (Y), t is 0.95 to 1.15, x is 0 to 0.3, y is 0.01 to 0.2, and the sum of x and y is less than 0.5.
[0151] Specific examples of NCA include LiNi 0.8 Co 0.15 Al 0.05 O 2 Examples include:
[0152] The content of the positive electrode active material is preferably 10% by mass or more, more preferably 30% by mass or more, even more preferably 50% by mass or more, and particularly preferably 70% by mass or more, based on the total amount of the positive electrode mixture layer. The content of the positive electrode active material is preferably 99.9% by mass or less, more preferably 99% by mass or less, based on the total amount of the positive electrode mixture layer.
[0153] (3.1.3.2) Binder Examples of binders include polyvinyl acetate, polymethyl methacrylate, nitrocellulose, fluororesin, and rubber particles. Examples of fluororesin include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), and vinylidene fluoride-hexafluoropropylene copolymer. Examples of rubber particles include styrene-butadiene rubber particles and acrylonitrile rubber particles. Among these, from the viewpoint of improving the oxidation resistance of the positive electrode mixture layer, it is preferable that the binder contains a fluororesin. Binders may be used alone or in combination of two or more. The content of the binder is preferably 0.1% by mass to 4% by mass relative to the total amount of the positive electrode mixture layer, from the viewpoint of achieving both the physical properties of the positive electrode mixture layer (e.g., electrolyte permeability, peel strength, etc.) and battery performance.
[0154] (3.1.3.3) Conductive Aid The positive electrode mixture layer may further contain a conductive aid. Known conductive aids can be used as the conductive aid. As the known conductive aid, conductive carbon materials are preferred. Examples of conductive carbon materials include graphite, carbon black, conductive carbon fiber, and fullerene. Examples of conductive carbon fibers include carbon nanotubes, carbon nanofibers, and carbon fibers. Examples of graphite include artificial graphite and natural graphite. Examples of natural graphite include flake graphite, lump graphite, and amorphous graphite. The conductive aids may be used alone or in combination of two or more. The material of the conductive aid may be a commercially available product.
[0155] (3.1.3.4) Other Components The positive electrode mixture layer may contain other components, such as a thickener, a surfactant, a dispersant, a wetting agent, and an antifoaming agent.
[0156] (3.2) Negative Electrode The negative electrode of the present disclosure includes a current collector (hereinafter also referred to as "negative electrode current collector") and a mixture layer (hereinafter also referred to as "negative electrode mixture layer"), and may also include an undercoat layer.
[0157] The negative electrode of the present disclosure may include a first negative electrode configuration, a second negative electrode configuration, a third negative electrode configuration, and a fourth negative electrode configuration. The first negative electrode configuration refers to a configuration in which an undercoat layer and a negative electrode composite layer are laminated in this order on both main surfaces of a current collector. The second negative electrode configuration refers to a configuration in which an undercoat layer and a negative electrode composite layer are laminated in this order on one main surface of a current collector, and an undercoat layer is laminated on the other main surface of the current collector. The third negative electrode configuration refers to a configuration in which an undercoat layer and a negative electrode composite layer are laminated in this order on one main surface of a current collector, and a negative electrode composite layer is laminated on the other main surface of the current collector. The fourth negative electrode configuration refers to a configuration in which an undercoat layer and a negative electrode composite layer are laminated in this order on one main surface of a current collector, and neither the undercoat layer nor the negative electrode composite layer is laminated on the other main surface of the current collector.
[0158] (3.2.1) Negative Electrode Current Collector Examples of the material for the negative electrode current collector include copper, aluminum, nickel, stainless steel (SUS), and nickel-plated steel.
[0159] (3.2.2) Undercoat Layer The undercoat layer is the same as the undercoat layer exemplified for the positive electrode.
[0160] (3.2.3) Negative Electrode Mixture Layer The negative electrode mixture layer contains a negative electrode active material and a binder.
[0161] (3.2.3.1) Negative Electrode Active Material The negative electrode active material is not particularly limited as long as it is a material capable of absorbing and releasing lithium ions. The negative electrode active material is preferably at least one material selected from the group consisting of, for example, metallic lithium, lithium-containing alloys, metals or alloys capable of alloying with lithium, oxides capable of doping and dedoping lithium ions, transition metal nitrides capable of doping and dedoping lithium ions, and carbon materials capable of doping and dedoping lithium ions. Among these, the negative electrode active material is preferably a carbon material capable of doping and dedoping lithium ions (hereinafter referred to as "carbon material").
[0162] Examples of carbon materials include carbon black, activated carbon, graphite materials, and amorphous carbon materials. These carbon materials may be used alone or in combination. The form of the carbon material is not particularly limited and may be, for example, fibrous, spherical, or flaky. The particle size of the carbon material is not particularly limited and is preferably 5 μm to 50 μm, more preferably 20 μm to 30 μm. Examples of amorphous carbon materials include hard carbon, coke, mesocarbon microbeads (MCMB) calcined at 1500°C or less, and mesophase pitch carbon fiber (MCF). Examples of graphite materials include natural graphite and artificial graphite. Examples of artificial graphite include graphitized MCMB and graphitized MCF. The graphite material may contain boron. The graphite material may be coated with a metal or amorphous carbon. Examples of the metal coating the graphite material include gold, platinum, silver, copper, and tin. The graphite material may be a mixture of amorphous carbon and graphite.
[0163] (3.2.3.2) Binder Examples of the binder contained in the negative electrode mixture layer include the same binders as those exemplified as the binder contained in the positive electrode mixture layer. The binder contained in the negative electrode mixture layer may be the same as or different from the binder contained in the positive electrode mixture layer. The content of the binder contained in the negative electrode mixture layer is not particularly limited, and may be the same as the content of the binder exemplified as the binder contained in the positive electrode mixture layer.
[0164] (3.2.3.3) Conductive additive The negative electrode mixture layer preferably contains a conductive additive. Examples of the conductive additive include the same conductive additives as those exemplified as the conductive additives that can be contained in the positive electrode mixture layer.
[0165] (3.2.3.4) Other Components The negative electrode mixture layer may contain other components in addition to the above components. Examples of other components include a thickener, a surfactant, a dispersant, a wetting agent, and an antifoaming agent.
[0166] The electrode of the present disclosure preferably has a current collector, an undercoat layer, and a composite layer laminated in this order.
[0167] (4) Lithium-ion secondary battery The lithium-ion secondary battery of the present disclosure includes the electrode of the present disclosure. A lithium-ion secondary battery generally includes an outer casing, electrodes (positive and negative electrodes), a separator, and an electrolyte. The outer casing accommodates the electrodes (positive and negative electrodes), the separator, and the non-aqueous electrolyte.
[0168] Hereinafter, an example will be described in which the positive electrode and the negative electrode are the electrodes of the present disclosure.
[0169] (4.1) Exterior Body Examples of the exterior body include an exterior body including a laminate film, an exterior body consisting of a battery can and a battery can lid, etc. The shape of the exterior body is not particularly limited and may be appropriately selected depending on the application of the lithium-ion secondary battery, etc.
[0170] (4.2) Electrodes The electrodes include a positive electrode and a negative electrode. The positive electrode is capable of absorbing and releasing lithium ions. The negative electrode is capable of absorbing and releasing lithium ions. In the lithium ion secondary battery of the present disclosure, at least one of the positive electrode and the negative electrode is the electrode of the present disclosure. When one of the positive electrode and the negative electrode of the lithium ion secondary battery of the present disclosure is the electrode of the present disclosure, the other of the positive electrode and the negative electrode may be a known electrode used in lithium ion secondary batteries.
[0171] (4.3) Separator The separator separates the positive electrode and the negative electrode. Examples of the separator include a porous resin flat plate. Examples of materials for the porous resin flat plate include resins and nonwoven fabrics containing such resins. Examples of resins include polyethylene (PE), polypropylene (PP), polymethylpentene (PMP), polyester, cellulose, and polyamide. Among these, the separator is preferably a porous resin sheet having a single layer or multilayer structure. The porous resin sheet is mainly made of one or more polyolefin resins. The thickness of the separator is preferably 5 μm to 30 μm. The separator is preferably disposed between the positive electrode and the negative electrode.
[0172] (4.4) Nonaqueous Electrolyte The nonaqueous electrolyte contains an electrolyte and a nonaqueous solvent. (4.4.1) Electrolyte The electrolyte preferably contains at least one of a fluorine-containing lithium salt (hereinafter also referred to as a "fluorine-containing lithium salt") and a fluorine-free lithium salt.
[0173] Examples of the fluorine-containing lithium salt include inorganic acid anion salts and organic acid anion salts. Examples of the inorganic acid anion salt include lithium hexafluorophosphate (LiPF 6 ), lithium tetrafluoroborate (LiBF 4 ), lithium hexafluoroarsenate (LiAsF 6 ), or lithium hexafluorotantalate (LiTaF 6 Examples of organic acid anion salts include lithium trifluoromethanesulfonate (LiCF 3 SO 3 Among them, the fluorine-containing lithium salt is LiPF 6 is particularly preferred. Examples of fluorine-free lithium salts include lithium perchlorate (LiClO 4 ), lithium aluminum tetrachloride (LiAlCl 4 ), or lithium decachlorodecaborate (Li 2 B 10 Cl 10 ) are listed.
[0174] When the electrolyte contains a fluorine-containing lithium salt, the content of the fluorine-containing lithium salt is preferably 50% by mass to 100% by mass, more preferably 60% by mass to 100% by mass, and even more preferably 80% by mass to 100% by mass, based on the total amount of the electrolyte. 6 ), lithium hexafluorophosphate (LiPF 6 The content of the component (a) is preferably 50% by mass to 100% by mass, more preferably 60% by mass to 100% by mass, and even more preferably 80% by mass to 100% by mass, based on the total amount of the electrolyte.
[0175] When the non-aqueous electrolyte contains an electrolyte, the concentration of the electrolyte in the non-aqueous electrolyte is preferably 0.1 mol / L to 3 mol / L, more preferably 0.5 mol / L to 2 mol / L. 6 ), the non-aqueous electrolyte contains lithium hexafluorophosphate (LiPF 6 The concentration of the HCl HCl solution is preferably 0.1 mol / L to 3 mol / L, more preferably 0.5 mol / L to 2 mol / L.
[0176] (4.4.2) Nonaqueous Solvent The nonaqueous electrolyte generally contains a nonaqueous solvent. Examples of the nonaqueous solvent include cyclic carbonates, fluorine-containing cyclic carbonates, chain carbonates, fluorine-containing chain carbonates, aliphatic carboxylic acid esters, fluorine-containing aliphatic carboxylic acid esters, γ-lactones, fluorine-containing γ-lactones, cyclic ethers, fluorine-containing cyclic ethers, chain ethers, fluorine-containing chain ethers, nitriles, amides, lactams, nitromethane, nitroethane, sulfolane, trimethyl phosphate, dimethyl sulfoxide, and dimethyl sulfoxide phosphate. The nonaqueous solvent may be used alone or in combination of two or more.
[0177] Examples of cyclic carbonates include ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate (BC). Examples of fluorine-containing cyclic carbonates include fluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), and trifluoropropylene carbonate. Examples of chain carbonates include dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), and dipropyl carbonate (DPC). Examples of fluorine-containing chain carbonates include methyl 2,2,2-trifluoroethyl carbonate. Examples of aliphatic carboxylic acid esters include methyl formate, methyl acetate, methyl propionate, methyl butyrate, methyl isobutyrate, methyl trimethylbutyrate, ethyl formate, ethyl acetate, ethyl propionate, ethyl butyrate, ethyl isobutyrate, and ethyl trimethylbutyrate. Examples of fluorine-containing aliphatic carboxylic acid esters include methyl difluoroacetate, methyl 3,3,3-trifluoropropionate, ethyl difluoroacetate, and 2,2,2-trifluoroethyl acetate. Examples of γ-lactones include γ-butyrolactone and γ-valerolactone. Examples of cyclic ethers include tetrahydrofuran, 2-methyltetrahydrofuran, tetrahydropyran, 1,3-dioxolane, 4-methyl-1,3-dioxolane, 1,3-dioxane, and 1,4-dioxane. Examples of the chain ethers include 1,2-ethoxyethane (DEE), ethoxymethoxyethane (EME), diethyl ether, 1,2-dimethoxyethane, and 1,2-dibutoxyethane. Examples of the fluorine-containing chain ethers include HCF 2 CF 2 CH 2 OCF 2 CF 2 H, C.F. 3 CF 2 CH 2 OCF 2 CF2 H, HCF 2 CF 2 CH 2 OCF 2 CFHCF 3 , C.F. 3 CF 2 CH 2 OCF 2 CFHCF 3 , C 6 F 13 OCH 3 , C 6 F 13 O.C. 2 H 5 , C 8 F 17 OCH 3 , C 8 F 17 O.C. 2 H 5 , C.F. 3 CFHCF 2 CH (CH 3 ) OCF 2 CFHCF 3 , HCF 2 CF 2 OCH (C 2 H 5 ) 2 , HCF 2 CF 2 O.C. 4 H 9 , HCF 2 CF 2 OCH 2 CH(C 2 H 5 ) 2 , or HCF 2 CF 2 OCH 2 CH (CH 3 ) 2 Examples of the nitriles include acetonitrile, glutaronitrile, adiponitrile, methoxyacetonitrile, and 3-methoxypropionitrile. Examples of the amides include N,N-dimethylformamide. Examples of the lactams include N-methylpyrrolidinone, N-methyloxazolidinone, and N,N'-dimethylimidazolidinone.
[0178] The non-aqueous solvent preferably contains at least one selected from the group consisting of cyclic carbonates, fluorine-containing cyclic carbonates, chain carbonates, and fluorine-containing chain carbonates. In this case, the total proportion of the cyclic carbonates, fluorine-containing cyclic carbonates, chain carbonates, and fluorine-containing chain carbonates is preferably 50% by mass to 100% by mass, more preferably 60% by mass to 100% by mass, and even more preferably 80% by mass to 100% by mass, based on the total amount of the non-aqueous solvent.
[0179] The non-aqueous solvent preferably contains at least one selected from the group consisting of cyclic carbonates and chain carbonates. In this case, the total amount of the cyclic carbonates and chain carbonates in the non-aqueous solvent is preferably 50% by mass to 100% by mass, more preferably 60% by mass to 100% by mass, and even more preferably 80% by mass to 100% by mass, based on the total amount of the non-aqueous solvent.
[0180] The content of the nonaqueous solvent is preferably 99% by mass or less, more preferably 97% by mass or less, and more preferably 90% by mass or less, based on the total amount of the nonaqueous electrolyte. The content of the nonaqueous solvent is preferably 60% by mass or more, and more preferably 70% by mass or more, based on the total amount of the nonaqueous electrolyte.
[0181] The intrinsic viscosity of the non-aqueous solvent is preferably 10.0 mPa·s or less at 25° C., from the viewpoint of further improving the dissociation property of the electrolyte and the mobility of ions.
[0182] (4.4.3) Electrolyte Additives The non-aqueous solvent may contain an electrolyte additive. This can make it difficult for side reactions that are not the original battery reaction to proceed during the charge / discharge cycle of the lithium-ion secondary battery. The battery reaction is a reaction in which lithium ions enter and exit (intercalate) the positive electrode and the negative electrode. Side reactions include a reductive decomposition reaction of the non-aqueous electrolyte by the negative electrode, an oxidative decomposition reaction of the non-aqueous electrolyte by the positive electrode, and elution of metal elements in the positive electrode active material. There are no particular limitations on the electrolyte additive, and any known additive can be used. For example, the additives described in JP 2019-153443 A can be used.
[0183] (5) Example of Lithium-ion Secondary Battery An example of a lithium-ion secondary battery according to an embodiment of the present disclosure will be specifically described with reference to Fig. 1 and Fig. 2. Fig. 1 is a schematic cross-sectional view of a lithium-ion secondary battery 1 according to an embodiment of the present disclosure. Fig. 2 is a schematic cross-sectional view of a positive electrode 11 in a lithium-ion secondary battery 1 according to an embodiment of the present disclosure. Fig. 3 is a schematic cross-sectional view of a negative electrode 12 in a lithium-ion secondary battery 1 according to an embodiment of the present disclosure.
[0184] A lithium-ion secondary battery 1 according to an embodiment of the present disclosure is a laminated type. As shown in FIG. 1 , the lithium-ion secondary battery 1 includes a battery element 10, a positive electrode lead 21, a negative electrode lead 22, and an exterior body 30. The battery element 10 is enclosed inside the exterior body 30. The exterior body 30 is formed of a laminate film. The positive electrode lead 21 and the negative electrode lead 22 are attached to the battery element 10. The positive electrode lead 21 and the negative electrode lead 22 are led out in opposite directions, from the inside to the outside of the exterior body 30.
[0185] As shown in FIG. 1 , the battery element 10 is formed by laminating a positive electrode 11, a separator 13, and a negative electrode 12. As shown in FIG. 2 , the positive electrode 11 is formed by forming positive electrode composite layers 11B on both main surfaces of a positive electrode current collector 11A with an undercoat layer. The positive electrode current collector 11A with an undercoat layer is formed by forming undercoat layers 111 on both main surfaces of a positive electrode current collector 110. As shown in FIG. 3 , the negative electrode 12 is formed by forming negative electrode composite layers 12B on both main surfaces of a negative electrode current collector 12A with an undercoat layer. The negative electrode current collector 12A with an undercoat layer is formed by forming undercoat layers 121 on both main surfaces of a negative electrode current collector 120. As shown in FIG. 1 , a positive electrode composite layer 11B formed on one main surface of an undercoat layer-attached positive electrode current collector 11A of a positive electrode 11 and a negative electrode composite layer 12B formed on one main surface of an undercoat layer-attached negative electrode current collector 12A of a negative electrode 12 adjacent to the positive electrode 11 face each other via a separator 13.
[0186] A non-aqueous electrolyte solution is poured into the interior of exterior body 30. The non-aqueous electrolyte solution permeates positive electrode composite layer 11B, separator 13, and negative electrode composite layer 12B. In lithium-ion secondary battery 1, one cell layer 14 is formed by adjacent positive electrode composite layer 11B, separator 13, and negative electrode composite layer 12B.
[0187] In the present embodiment, the lithium ion secondary battery 1 is a stacked type, but the present disclosure is not limited thereto. The lithium ion secondary battery 1 may be, for example, a wound type. The wound type is formed by stacking a positive electrode, a separator, a negative electrode, and a separator in this order and winding them into layers. The wound type includes a cylindrical type and a rectangular type. In the present embodiment, as shown in FIG. 1 , the directions in which the positive electrode lead 21 and the negative electrode lead 22 protrude from the inside of the exterior body 30 to the outside are opposite directions relative to the exterior body 30, but the present disclosure is not limited thereto. For example, the directions in which the positive electrode lead and the negative electrode lead protrude from the inside of the exterior body 30 to the outside may be the same direction relative to the exterior body 30.
[0188] Hereinafter, embodiments of the present disclosure will be described in detail with reference to examples, but the present disclosure is not limited to the descriptions of these examples.
[0189] [1] Preparation The products used in the examples and comparative examples are as follows. The physical properties of each product are catalog values.
[0190] [1.1] Conductive carbon material (A) Super-P: "Super-P" manufactured by TIMCAL (conductive carbon black, solid content: 100% by mass) KS-6: "KS-6" manufactured by TIMREX (flake graphite, solid content: 100% by mass)
[0191] [1.2] Olefin-based resins (B) W300: "Chemipearl (registered trademark) W300" manufactured by Mitsui Chemicals, Inc. (water dispersion of low molecular weight polyethylene, solid content: 40% by mass, particle size (average primary particle size measured by the Cole counter method; the same applies hereinafter): 3.0 μm, softening point (ring and ball method): 132°C) W700: "Chemipearl (registered trademark) W700" manufactured by Mitsui Chemicals, Inc. (water dispersion of low molecular weight polyethylene, solid content: 40% by mass, particle size: 1.0 μm, softening point (ring and ball method): 132°C) W900: "Chemipearl (registered trademark) W900" manufactured by Mitsui Chemicals, Inc. (water dispersion of low molecular weight polyethylene, solid content: 40% by mass, particle size: 0.6 μm, softening point (ring and ball method): 132°C) W950: "Chemipearl (registered trademark)" manufactured by Mitsui Chemicals, Inc. W950 (water dispersion of low molecular weight polyethylene, solid content: 40% by mass, particle size: 0.6 μm, softening point (ring and ball method): 113° C.) WP100: "CHEMIPEARL (registered trademark) WP100" manufactured by Mitsui Chemicals, Inc. (water dispersion of low molecular weight polypropylene, solid content: 40% by mass, particle size: 1.0 μm, softening point (ring and ball method): 148° C.)
[0192] [1.3] Water-soluble acrylic polymer (C) As the water-soluble acrylic polymer (C), water-soluble acrylic polymer (C-1) to water-soluble acrylic polymer (C-5') were prepared as follows.
[0193] [1.3.1] Acrylic Water-Soluble Polymer (C-1) 240.0 parts by mass of distilled water was charged into a separable flask equipped with a stirrer and reflux condenser, and after purging with nitrogen gas, the temperature was raised to 70°C. Next, 0.6 parts by mass of ammonium persulfate was added, and the following water-soluble monomer raw materials were continuously added over 3 hours. The mixture was maintained for another 3 hours, and the pH was adjusted to 9.0 with aqueous ammonia to complete the polymerization. An appropriate amount of water was added to obtain an aqueous solution of acrylic water-soluble polymer (C-1). The solids content of the aqueous solution of acrylic water-soluble polymer (C-1) was 15.0%.
[0194] <Water-soluble monomer raw material> Methacrylamide 40.0 parts by mass Methacrylic acid 50.0 parts by mass 2-hydroxyethyl methacrylate 10.0 parts by mass 25% aqueous ammonia 50.0 parts by mass Distilled water 240.0 parts by mass
[0195] [1.3.1.2] Glass transition temperature (Tg) The glass transition temperature (Tg) of the acrylic water-soluble polymer (C-1) contained in the obtained aqueous solution was calculated using the FOX formula shown below (1). Formula (1): 1 / Tg=W1 / Tg1+W2 / Tg2+ ... +Wn / Tgn In formula (1), Tg is the glass transition temperature of the copolymer (unit: K), Tgi (i = 1, 2, ... n) is the glass transition temperature (unit: K) when monomer i forms a homopolymer, and Wi (i = 1, 2, ... n) is the mass fraction of monomer i in all monomers.
[0196] [1.3.2] Aqueous solutions of acrylic water-soluble polymer (C-2) to acrylic water-soluble polymer (C-5') were produced in the same manner as in Example 1, except that the blending formulation was changed according to the description in Table 1. The glass transition temperatures of acrylic water-soluble polymer (C-2) to acrylic water-soluble polymer (C-5') were determined in the same manner as in Example 1.
[0197]
[0198] In Table 1, "240 / 240" indicates that 240 parts by mass of distilled water was initially charged into the flask, and then 240 parts by mass of distilled water was used when dissolving the monomer.
[0199] [1.3.3] Comparative Resins for Acrylic Water-Soluble Polymer (C) The following resins were prepared as comparative resins for the acrylic water-soluble polymer (C): Polyacrylic acid: "Polyacrylic acid" manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. (aqueous polyacrylic acid solution, solids concentration: approximately 25% by mass); Polyacrylamide: "Polyacrylamide" manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. (aqueous polyacrylamide solution, solids concentration: approximately 10% by mass).
[0200] [1.4] Additives (D) CMC: "2200" manufactured by Daicel Miraize Co., Ltd. (sodium carboxymethylcellulose, solid content: 100% by mass) PVDF: "W#7200" manufactured by Kureha Corporation (vinylidene fluoride resin, solid content: 100% by mass) SBR: "TRD2001" manufactured by JSR Corporation (aqueous dispersion of styrene butadiene rubber particles, solid content: 50% by mass) MC: "Matsumoto Microsphere (registered trademark) FN-100SS" manufactured by Matsumoto Yushi Pharmaceutical Co., Ltd. (microcapsules, solid content: 100% by mass, maximum volume expansion temperature: 145 to 155°C, volume expansion starting temperature: 120 to 130°C) Al 2 O 3 :Fujifilm Wako Pure Chemical Industries, Ltd. "Aluminum oxide" (average particle size: 2 μm, solid content: 100% by mass)
[0201] Specific numerical values of the blending ratios (content ratios), physical property values, parameters, etc. used in the following description can be replaced with the upper limit values (numerical values defined as "not more than" or "less than") or lower limit values (numerical values defined as "not less than" or "exceeding") of the corresponding blending ratios (content ratios), physical property values, parameters, etc. described in the above "Modes for Carrying Out the Invention." Furthermore, unless otherwise specified in the following description, "parts" and "%" are based on mass.
[0202] [2] Preparation of Positive Electrode Current Collector with Undercoat Layer [2.1] Preparation of Slurry for Undercoat Layer (Example 1) A 5 L planetary dispersion was used to prepare the slurry for the undercoat layer. A three-roll mill (BR-300HCVIII, manufactured by Imex Co., Ltd.) was used to disperse the slurry for the undercoat layer. 58 parts by mass of "Super-P" (A) were pre-mixed for 5 minutes (Preparation Step A). 229.0 parts by mass of "CMC aqueous solution" (D) were added to the "Super-P" (A) powder and mixed for an additional 20 minutes to obtain a first mixture (Preparation Step B). The "CMC aqueous solution" (D) was prepared by adding "CMC" (D) to distilled water so that the content of "CMC" (D) was 1.6% by mass relative to the total amount of "CMC aqueous solution" (D). To the first mixed solution, 527.8 parts by mass of "CMC aqueous solution" (D) was added and mixed for 20 minutes. This addition operation was performed three times to obtain a second mixed solution (Preparation step C). The total amount of "CMC aqueous solution" (D) added to the first mixed solution was 1583.4 parts by mass. To the second mixed solution, 95.4 parts by mass of "acrylic water-soluble polymer (C-1)" (C) and 471.3 parts by mass of "W700" (B) were added, kneaded for 20 minutes, and vacuum degassed for 30 minutes to obtain a third mixed solution (Preparation step D). The third mixed solution was dispersed twice using the three-roll mill shown in FIG. 4 under conditions of a roll gap of 10 μm and a roll rotation speed of 300 rpm (gear ratio 1:3:9) (Preparation step E). That is, the rotation speed of the charge roll 91 was 33.3 rpm, the rotation speed of the intermediate roll 92 was 100 rpm, the rotation speed of the finishing roll 93 was 300 rpm, the first gap L1 was 10 μm, and the second gap L2 was 10 μm. In this way, a slurry (composition) for the undercoat layer having a solid content concentration of 12.4 mass% was prepared (preparation step E).
[0203] (Examples 2 to 8, Example 11, Comparative Examples 1 to 5) Slurries (compositions) for the undercoat layer were prepared in the same manner as in Example 1, except that the additive materials and amounts added in each of Preparation Steps A to D were changed as shown in Table 2.
[0204]
[0205] In Table 2, "WSP" represents an acrylic water-soluble polymer, "PA" represents polyacrylic acid, and "PAA" represents polyacrylamide.
[0206] (Example 9) A 5 L planetary dispenser was used to prepare the slurry for the undercoat layer. A three-roll mill (BR-300HCVIII, manufactured by Imex Co., Ltd.) was used to disperse the slurry for the undercoat layer. 58 parts by mass of "Super-P" (A) and "Al 2 O 3 " (D) 87.0 parts by mass were mixed for 10 minutes to obtain a mixture (preparation step A). 550.0 parts by mass of "CMC aqueous solution" (D) was added to the mixture and mixed for a further 20 minutes to obtain a first mixed solution (preparation step B). "CMC aqueous solution" (D) was prepared by adding "CMC" (D) to distilled water so that the content of "CMC" (D) was 1.0% by mass relative to the total amount of "CMC aqueous solution" (D). 300.0 parts by mass of "CMC aqueous solution" (D) was added to the first mixed solution and mixed for 20 minutes. This addition operation was performed three times to obtain a second mixed solution (preparation step C). The total amount of "CMC aqueous solution" (D) added to the first mixed solution was 900.0 parts by mass. To the second mixed solution, 95.4 parts by mass of "acrylic water-soluble polymer (C-3)" (C) and 290.0 parts by mass of "W700" (B) were added, and the mixture was kneaded for 20 minutes and vacuum degassed for 30 minutes to obtain a third mixed solution (preparation step D). The third mixed solution was dispersed twice using a three-roll mill shown in FIG. 4 under the conditions of a roll gap of 10 μm and a roll rotation speed of 300 rpm (gear ratio 1: 3: 9) (preparation step E). That is, the rotation speed of the charge roll 91 was 33.3 rpm, the rotation speed of the intermediate roll 92 was 100 rpm, the rotation speed of the finishing roll 93 was 300 rpm, the first gap L1 was 10 μm, and the second gap L2 was 10 μm. In this way, a slurry (composition) for the undercoat layer having a solids concentration of 14.9% by mass was prepared (preparation step E).
[0207] Example 10 A slurry (composition) for an undercoat layer was prepared in the same manner as in Example 9, except that the additive materials in the preparation step A were changed as shown in Table 3.
[0208]
[0209] In Table 3, "WSP" represents an acrylic water-soluble polymer.
[0210] [2.2] Coating and drying of undercoat layer A die coater was used to coat the slurry for the undercoat layer. After drying, the coating thickness was 3 μm (coating weight was approximately 0.2 mg / cm 2 The undercoat layer slurry was applied to one main surface of an aluminum foil (thickness 20 μm, width 200 mm, positive electrode current collector) and dried so that the thickness after drying was 3 μm. Next, the undercoat layer slurry was similarly applied to the other main surface (uncoated surface) of the aluminum foil and dried so that the thickness after drying was 3 μm. In this way, an aluminum foil roll (positive electrode current collector with undercoat layer) was obtained, with undercoat layers coated on both sides.
[0211] [3] Preparation of Positive Electrode [3.1] Preparation of Positive Electrode Mixture Slurry A 5 L planetary dispenser was used to prepare the positive electrode mixture slurry. 0.5 Co 0.2 Mn 0.3 O 2 ) 1520 parts by mass of conductive additive "Super-P" (conductive carbon manufactured by TIMCAL Corporation) 30 parts by mass of conductive additive "KS-6" (flake graphite manufactured by TIMREX Corporation) 30 parts by mass of conductive additive were mixed for 10 minutes to obtain a positive electrode mixture. 50 parts by mass of "NMP" was added to the positive electrode mixture and mixed for 20 minutes to obtain a first positive electrode mixture. 350 parts by mass of "PVDF solution" was added to the first positive electrode mixture and kneaded for 30 minutes, and then 260 parts by mass of "PVDF solution" was added and kneaded for 15 minutes, and then 220 parts by mass of "PVDF solution" was added and kneaded for 15 minutes to obtain a second positive electrode mixture. The "PVDF solution" was prepared by adding "PVDF" to "NMP" so that the "PVDF" content was 8 mass % relative to the total amount of the "PVDF solution." To adjust the viscosity, 80 parts by mass of "NMP" was added to the second positive electrode mixture and mixed for 30 minutes, followed by vacuum degassing for 30 minutes. In this way, a positive electrode mixture slurry with a solid content concentration of 65 mass % was prepared.
[0212] [3.2] Coating and Drying A die coater was used to coat the positive electrode mixture slurry. The mass of the positive electrode mixture layer (coated film after drying) was 19.0 mg / cm 2 The positive electrode composite slurry was applied to one main surface (i.e., the undercoat layer) of a positive electrode current collector with an undercoat layer (aluminum foil thickness: 20 μm, thickness of one undercoat layer: 3 μm, width: 200 mm) and dried so that the mass of the positive electrode composite layer (coated film after drying) became 19.0 mg / cm 2 The positive electrode mixture slurry was similarly applied to the other main surface (i.e., the undercoat layer) of the positive electrode current collector with the undercoat layer so that the total coating amount on both sides was 38.0 mg / cm. 2 ) was dried in a vacuum drying oven at 130°C for 12 hours.
[0213] [3.3] Pressing A 35-ton press was used to press the positive electrode roll. The gap between the upper and lower rolls was adjusted to press the positive electrode to a density of 2.9±0.05 g / cm. 3 The mixture was pressed using a 35-ton press machine so that the thickness became
[0214] [3.4] Slitting The positive electrode roll was slit so as to obtain an area for the positive electrode composite layer (front surface: 56 mm × 334 mm, back surface: 56 mm × 408 mm) and an area for a tab welding margin, thereby obtaining a positive electrode in which an undercoat layer was laminated on the aluminum foil.
[0215] [4] Preparation of Negative Electrode [4.1] Preparation of Negative Electrode Mixture Slurry A 5 L planetary disperser was used to prepare the negative electrode mix slurry. 1050 parts by mass of "natural graphite" as the negative electrode active material and "Super-P" (conductive carbon, BET specific surface area 62 m) as the conductive additive were added. 211 parts by mass of PEG-100 / g) was mixed for 10 minutes to obtain a negative electrode mixture. 450 parts by mass of "CMC aqueous solution" was added to the negative electrode mixture and mixed for an additional 20 minutes to obtain a first negative electrode mixture. 150 parts by mass of "CMC aqueous solution" was added to the first negative electrode mixture and mixed for an additional 30 minutes, 293.5 parts by mass of "CMC aqueous solution" was added and mixed for 30 minutes, and 450 parts by mass of water as a solvent was added and mixed for 15 minutes to obtain a second negative electrode mixture. 45 parts by mass of "SBR aqueous solution" (manufactured by JSR Corporation, solid content concentration: 50% by mass) was added to the second negative electrode mixture and kneaded for 15 minutes, followed by vacuum degassing for 10 minutes. In this way, a negative electrode mixture slurry with a solid content concentration of 45% by mass was prepared.
[0216] [4.2] Coating and Drying A die coater was used to coat the negative electrode mixture slurry. The mass of the negative electrode mixture layer (coated film after drying) was 11.0 mg / cm 2 The negative electrode composite slurry was applied to one main surface of a copper foil (thickness 10 μm, negative electrode current collector) and dried. Then, the negative electrode composite slurry was similarly applied to the opposite surface (uncoated surface) so that the mass of the negative electrode composite layer (coated film after drying) became 11.0 mg / cm. 2 The negative electrode composite slurry was applied to the other main surface of the copper foil and dried. 2 ) was dried in a vacuum drying oven at 120°C for 12 hours.
[0217] [4.3] Pressing A small press was used to press the negative electrode roll. The gap between the upper and lower rolls was adjusted, and the negative electrode roll was pressed to a density of 1.45±0.05 g / cm. 3 The mixture was pressed using a small press to obtain a final product.
[0218] [4.4] Slitting The negative electrode roll was slit to obtain a negative electrode having an area for the negative electrode composite layer (front surface: 58 mm × 372 mm, back surface: 58 mm × 431 mm) and an area for a tab welding margin.
[0219] [5] Preparation of wound battery (design capacity 1 Ah) [5.1] Winding A polyethylene porous film (60.5 mm x 450 mm) with a porosity of 45% by volume and a thickness of 25 μm was used as the separator. The negative electrode, separator, positive electrode with an undercoat layer, and separator obtained above were stacked and wound, and then press-molded. Next, an aluminum tab was bonded to the margin of the positive electrode with the undercoat layer using an ultrasonic bonding machine, and a nickel tab was bonded to the margin of the negative electrode using an ultrasonic bonding machine. This was sandwiched between laminate films, and three sides were heat-sealed. This resulted in an exterior body with an opening (hereinafter referred to as the "first exterior body").
[0220] [5.2] Injection of non-aqueous electrolyte Ethylene carbonate (EC), methyl ethyl carbonate (EMC), and dimethyl carbonate (DMC) were mixed in a volume ratio of EC:EMC:DMC=3:3:4 to obtain a mixed solvent. 6 A non-aqueous electrolyte was prepared by dissolving the non-aqueous electrolyte in a vacuum dryer at a concentration of 1.0 mol / L. Before the non-aqueous electrolyte solution was poured into the first outer casing, the first outer casing was dried under reduced pressure at 70°C for 12 hours. After pouring 4.7±0.1 g of the electrolyte solution into the first outer casing, the opening of the first outer casing was heat-sealed while drawing a vacuum. This produced a lithium-ion secondary battery precursor.
[0221] [5.3] Activation Treatment The lithium ion secondary battery precursor was maintained at room temperature (25°C) for 24 hours. Next, the lithium ion secondary battery precursor was charged at a constant current of 0.05C (0.05C-CC) for 4 hours, followed by a 12-hour pause. Thereafter, it was charged at a constant current and constant voltage of 0.1C (0.1C-CCCV) to 4.2V, paused for 30 minutes, and then discharged at a constant current of 0.1C (0.1C-CCCV) to 2.8V. Furthermore, a charge-discharge cycle (charging to 4.2V at 0.1C-CCCV and discharging to 2.8V at 0.1C-CC) was repeated five times. The lithium ion secondary battery precursor was then stored at 25°C for five days in a fully charged state of 4.2V (SOC 100%). In this manner, wound-type batteries (lithium ion secondary batteries) of Examples 1 to 11, Comparative Examples 1 to 5, and Reference Example were obtained.
[0222] [6] Evaluation Method The following particle size distribution measurements were performed on the slurries for the undercoat layer prepared in Examples 1 to 11 and Comparative Examples 1 to 5. The following safety (heating), safety (nail penetration), initial DCIR, and DCIR after high-temperature storage were evaluated on the wound-type batteries of Examples 1 to 11, Comparative Examples 1 to 5, and the Reference Example. The evaluation results are shown in Table 5.
[0223] [6.1] Particle Size Distribution 1.0 g of the undercoat layer slurry (hereinafter also referred to as "sample") of Examples 1 to 11 and Comparative Examples 1 to 5 and 50 ml of water were placed in a 100 ml beaker, the sample lumps were crushed with a spatula, and the mixture was gently mixed with a dropper. Next, the sample was dispersed in water using a tabletop ultrasonic cleaner (Honda Electronics Co., Ltd., Model W-113). The tabletop ultrasonic cleaner was set to an output of 100 W and 28 kHz, and the dispersion was carried out for 60 seconds. After that, bubbles formed on the surface of the aqueous solution in the beaker were removed, and the volume-based particle size distribution of the sample was measured using a particle size distribution analyzer (Microtrac MT3300EXII, Microtrac-Bell Co., Ltd.) by laser light diffraction scattering. From this measurement, the D10, D50, D90, and D99 in the volume particle size distribution were determined. The measurement results for D10, D50, D90 and D99 are shown in Table 5.
[0224] [6.2] Safety (heating) A wound-type battery (design capacity 1 Ah) was charged at a constant current and constant voltage (0.1 C-CCCV) to 4.2 V at 0.1 C in a temperature environment of 25 ° C, and safety (heating) was evaluated. The measurement cell was placed in a thermostatic bath heated to 50 ° C, and the AC resistance was measured at 1 kHz (amplitude 10 mV) while the temperature of the thermostatic bath was raised at 5 ° C / min. The cell temperature was recorded using a temperature measurement terminal installed on the top surface of the cell. The AC resistance was measured using a ModuLab XM ECS electrochemical measurement system manufactured by Solartron.
[0225] The resistance rise starting temperature and resistance change ratio were calculated from the measured resistance value. The resistance rise starting temperature was calculated as the temperature at which the resistance value reached 1.5 times the resistance value at 50°C, which was set to 1. The resistance change ratio was calculated as the relative ratio of the resistance value at 150°C to the resistance value at 50°C, which was set to 1.
[0226] Using the measurement results of the resistance rise starting temperature and the resistance change ratio, the safety (heating) was evaluated according to the following criteria: Acceptable evaluations of safety (heating) are "A" and "B".
[0227] A: The resistance rise starting temperature is 90°C or less, and the resistance change ratio is 20 times or more. B: The resistance rise starting temperature is over 90°C, and the resistance change ratio is 20 times or more. Or the resistance rise starting temperature is 90°C or less, and the resistance change ratio is less than 20 times. C: The resistance rise starting temperature is over 90°C, and the resistance change ratio is less than 20 times.
[0228] [6.3] Forced Internal Short Circuit Test (Nail Penetration Test) A wound battery (design capacity 1 Ah) was charged at a constant current and constant voltage (0.1 C-CCCV) to 4.2 V at 0.1 C in a temperature environment of 25°C, and a nail penetration test (nail diameter 3 mm, nail penetration rate 1.0 mm / sec) was performed. A nail with a diameter of 3 mm was inserted into the center of the wound battery (cell) at a rate of 1.0 mm / sec, short-circuiting the positive and negative electrodes inside the battery container. The short-circuit behavior of the battery at this time was observed. The nail penetration test was performed on multiple batteries (3 to 6 times) at the same level, and the total number of test batteries was evaluated according to the following criteria. Acceptable ratings for the nail penetration test were "A" and "B."
[0229] A: The percentage of batteries whose internal temperature exceeded 300°C was less than 10% of the total number of test batteries. B: The percentage of batteries whose internal temperature exceeded 300°C was more than 10% and less than 60% of the total number of test batteries. C: The percentage of batteries whose internal temperature exceeded 300°C was 60% or more of the total number of test batteries.
[0230] [6.4] Initial DCIR Evaluation [6.4.1] Initial DCIR Measurement A wound battery (design capacity 1 Ah) was subjected to a constant current / constant voltage charge (0.1C-CCCV) at 0.1C to 4.2V in a temperature environment of 25°C, and initial DCIR measurement was performed. The battery was then subjected to a constant current discharge at 0.1C for 10 seconds (0.1C-CC-10s) and a constant current charge at 0.1C for 10 seconds (0.1C-CC-10s). The battery was then subjected to a constant current discharge at 0.2C for 10 seconds (0.2C-CC-10s) and a constant current charge at 0.2C for 10 seconds (0.2C-CC-10s). The battery was then subjected to a constant current discharge at 0.5C for 10 seconds (0.5C-CC-10s) and a constant current charge at 0.5C for 10 seconds (0.5C-CC-10s). Next, the battery was subjected to a constant current discharge at 1.0 C for 10 seconds (1.0 C-CC-10 s), followed by a constant current charge at 1.0 C for 10 seconds (1.0 C-CC-10 s). It was then subjected to a constant current discharge at 2.0 C for 10 seconds (2.0 C-CC-10 s), followed by a constant current charge at 2.0 C for 10 seconds (2.0-CC-10 s). The first DC resistance (DCIR) was calculated based on the voltage drop (= voltage before discharge start - voltage 10 seconds after discharge start) due to "CC10s discharge" at each discharge rate of 0.1 C to 2.0 C, and each current value (i.e., each current value corresponding to a discharge rate of 0.1 C to 2.0 C).
[0231] [6.4.2] Evaluation method Based on the above measured values, a first relative value was calculated by setting the measured value of the first direct current resistance (DCIR) of the reference example (without undercoat layer) as 100, and initial DCIR evaluation was performed according to the following criteria. The first relative values of the first direct current resistance are shown in Table 5. Acceptable evaluations of the initial DCIR evaluation are "A" and "B".
[0232] A: The first relative value is 100 or less. B: The first relative value is more than 100 and is 105 or less. C: The first relative value is more than 105.
[0233] [6.5] DCIR Evaluation After High-Temperature Storage [6.5.1] DCIR Measurement After High-Temperature Storage The fabricated wound battery (design capacity 1 Ah) was charged at 0.1 C to 4.2 V at a constant current and constant voltage (0.1 C-CCCV) in a temperature environment of 25°C, and then left in a charged state in an atmosphere of 60°C for 28 days. In this way, a battery after high-temperature storage was obtained. The same DCIR evaluation process as the initial DCIR evaluation process described above was performed, and the second DC resistance (DCIR) was determined.
[0234] [6.5.2] Evaluation method Based on the above measured values, a second relative value was calculated by setting the measured value of the second direct current resistance (DCIR) of the reference example (without undercoat layer) as 100, and the DCIR after high-temperature storage was evaluated according to the following criteria. The second relative values of the second direct current resistance are shown in Table 5. Acceptable evaluations of the DCIR after high-temperature storage are "A" and "B".
[0235] A: The second relative value is 105 or less. B: The second relative value is greater than 105 and less than 110. C: The second relative value is greater than 110.
[0236]
[0237]
[0238] In Tables 4 and 5, "MA" indicates a constitutional unit derived from methacrylamide. "COOH" indicates a constitutional unit derived from a vinyl monomer having a carboxy group. "OH" indicates a constitutional unit derived from a vinyl monomer having a hydroxyl group. "Onset temperature" indicates the temperature at which resistance rise begins. "Change ratio" indicates the resistance change ratio. "Initial" indicates the initial DCIR evaluation. "After high-temperature storage" indicates the DCIR evaluation after high-temperature storage. "PA" indicates polyacrylic acid. "PAA" indicates polyacrylamide.
[0239] The acrylic water-soluble polymers (C) of Comparative Examples 1 to 5 did not satisfy the requirements that the content of structural units derived from (meth)acrylamide be 35% (30% by mass) to 95% by mass, relative to the total amount of the acrylic water-soluble polymer (C), and that the content of structural units derived from vinyl monomer be 5% (70% by mass), relative to the total amount of the acrylic water-soluble polymer (C). Therefore, in Comparative Example 1, the evaluation result of the DCIR evaluation after high-temperature storage was "C". In Comparative Examples 2 and 4, the evaluation results of the initial DCIR evaluation and the DCIR evaluation after high-temperature storage were "C". In Comparative Example 3, the evaluation results of the safety (heating), safety (nail penetration), initial DCIR evaluation, and DCIR evaluation after high-temperature storage were "C". In Comparative Example 5, the evaluation results of the safety (nail penetration), initial DCIR evaluation, and DCIR evaluation after high-temperature storage were "C". These results show that the compositions of Comparative Examples 1 to 5 are not suitable for forming electrodes that are safe, have low DC resistance during initial charge / discharge, and are inhibited from increasing in DC resistance under high-temperature conditions (especially after long-term storage).
[0240] The compositions of Examples 1 to 11 contained a conductive carbon material (A), an olefin resin (B), and an acrylic water-soluble polymer (C). The acrylic water-soluble polymer (C) satisfied the following conditions: the content of structural units derived from (meth)acrylamide was 35% (30% by mass) to 95% by mass, relative to the total amount of the acrylic water-soluble polymer (C); and the content of structural units derived from vinyl monomers was 5% (70% by mass), relative to the total amount of the acrylic water-soluble polymer (C). Therefore, in Examples 1 to 11, the evaluation results for safety (heating), safety (nail penetration), initial DCIR evaluation, and DCIR evaluation after high-temperature storage were "A" or "C." From these results, it was found that the compositions of Examples 1 to 11 were excellent in safety, had low DC resistance during initial charge and discharge, and were suitable for forming electrodes in which the increase in DC resistance in high-temperature environments (particularly after long-term storage) was suppressed.
[0241] The disclosure of Japanese Patent Application No. 2023-052346, filed on March 28, 2023, is incorporated herein by reference in its entirety. All documents, patent applications, and technical standards described herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard was specifically and individually indicated to be incorporated by reference.
Claims
1. A composition comprising a conductive carbon material (A), an olefin resin (B) and an acrylic water-soluble polymer (C), wherein the acrylic water-soluble polymer (C) has structural units derived from (meth)acrylamide and structural units derived from a vinyl monomer having at least one of a carboxy group and a hydroxyl group, the content of the structural units derived from the (meth)acrylamide being 35% by mass to 95% by mass relative to the total amount of the acrylic water-soluble polymer (C), and the content of the structural units derived from the vinyl monomer having at least one of a carboxy group and a hydroxyl group being 5% by mass to 65% by mass relative to the total amount of the acrylic water-soluble polymer (C).
2. The composition according to claim 1, wherein the content of the conductive carbon material (A) is 1% by mass to 30% by mass, based on the total amount of the composition, the content of the olefin resin (B) is 30% by mass to 90% by mass, based on the total amount of the composition, and the content of the acrylic water-soluble polymer (C) is 1% by mass to 20% by mass, based on the total amount of the composition.
3. The composition according to claim 1, wherein the olefin-based resin (B) comprises an ethylene-based resin or a propylene-based resin.
4. The composition according to claim 1, wherein the particle size of said olefin-based resin (B) is 0.1 μm to 9.0 μm, and the softening point of said olefin-based resin (B) is 70° C. or higher.
5. The composition according to claim 1, wherein the water-soluble acrylic polymer (C) has a structural unit derived from (meth)acrylamide, a structural unit derived from a vinyl monomer having a carboxy group, and a structural unit derived from a vinyl monomer having a hydroxyl group.
6. The composition according to claim 1, wherein the Tg of the acrylic water-soluble polymer (C) is 150° C. or higher.
7. The composition according to claim 1, further comprising an additive (D), the content of said additive (D) being 1 mass % to 50 mass % based on the total amount of the composition.
8. The composition of claim 7, wherein the additive (D) comprises carboxymethyl cellulose.
9. The composition according to claim 7, wherein the additive (D) comprises at least one of a thermally expandable microcapsule having a maximum volume expansion temperature of 70°C to 180°C and an inorganic oxide filler.
10. The composition according to claim 1, having a ratio of particle size distribution D99 to particle size distribution D10 (D99 / D10) of 35 or less, as measured by a laser light diffraction scattering method.
11. The composition according to claim 1, having a particle size distribution D99 measured by a laser light diffraction scattering method of 20 μm or less.
12. The composition according to claim 1, wherein the ratio of particle size distribution D99 to particle size distribution D50 (D99 / D50) measured by a laser light diffraction scattering method is 20 or less.
13. An undercoat layer comprising the composition according to any one of claims 1 to 12.
14. An electrode comprising a current collector, the undercoat layer according to claim 13, and a composite layer.
15. The electrode according to claim 14, wherein the current collector, the undercoat layer, and the composite layer are laminated in this order.
16. A lithium ion secondary battery comprising the electrode according to claim 14.
Citation Information
Patent Citations
Binder for carbon coat foil coating solution, carbon coat foil coating solution, carbon coat foil, electrode for lithium ion secondary battery, and lithium ion secondary battery
JP2013229187A
Aqueous solution of thermally crosslinkable binder for lithium ion battery, electrode slurry for lithium ion battery and manufacturing method thereof, electrode for lithium ion battery, and lithium ion battery
JP2020024896A
PTC functional composition, PTC functional composition layer, coated current collector for non-aqueous electrolyte secondary battery, electrode for non-aqueous electrolyte secondary battery, and non-aqueous electrolyte secondary battery
JP2023147402A
Positive electrode equipped with undercoat layer containing microcapsules, and lithium-ion secondary battery
WO2019189866A1
Cited By
Electrode composition, undercoat layer, electrode, and lithium-ion secondary battery
JP2026156385A