Platinum-phosphite complex-containing hydrosilylation catalyst, method for producing said platinum-phosphite complex-containing hydrosilylation catalyst, and curable organopolysiloxane composition containing said catalyst

WO2024219089A1PCT designated stage expired Publication Date: 2024-10-24SHIN ETSU CHEMICAL CO LTD

Patent Information

Application Number
PCT/JP2024/007309
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-21
Filing Date
2024-02-28
Publication Date
2024-10-24

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

The present invention pertains to: a platinum-phosphite complex-containing hydrosilylation catalyst that is liquid at 23°C and that is characterized by not containing a hydrocarbon-based organic solvent and by being obtained through association of a platinum-phosphite ester complex and a silane compound and / or a partial hydrolysate thereof; and a method for producing the platinum-phosphite complex-containing hydrosilylation catalyst. Accordingly, provided is a platinum-phosphite complex-containing hydrosilylation catalyst that does not contain an organic solvent and that is liquid at 23°C.
Need to check novelty before this filing date? Find Prior Art

Description

Platinum-phosphite complex-containing hydrosilylation catalyst, method for producing said platinum-phosphite complex-containing hydrosilylation catalyst, and curable organopolysiloxane composition containing said catalyst

[0001] The present invention relates to a platinum-phosphite complex-containing hydrosilylation catalyst, a curable organopolysiloxane composition using the catalyst, and a method for producing the platinum-phosphite complex-containing hydrosilylation catalyst.

[0002] The addition reaction curable organopolysiloxane composition contains an organohydrogenpolysiloxane having a hydrogen atom bonded to a silicon atom (i.e., a hydrosilyl group), an organopolysiloxane having an alkenyl group such as a vinyl group bonded to a silicon atom, and a platinum catalyst.

[0003] In the case of so-called one-component organopolysiloxane compositions in which these three components are combined into one composition, exposure to high temperature conditions can result in problems such as changes in properties such as thickening and gelation, and changes in the physical properties of the organopolysiloxane cured product obtained after curing. To avoid these problems, methods have been used in which the components are divided into two or more components and mixed immediately before use to form a mixed organopolysiloxane composition, or in which the one-component organopolysiloxane composition is transported refrigerated or frozen.

[0004] In the former case, there is a concern that the physical properties of the resulting organopolysiloxane cured product may change due to blending or mixing, requiring highly advanced blending and mixing techniques. Meanwhile, in the latter case, refrigeration or freezing conditions are required from storage until use, resulting in extremely high transportation and storage costs, making it commercially disadvantageous. Against this background, there has been a growing demand in recent years for one-component organopolysiloxane compositions whose properties and performance do not change even when stored for long periods at room temperature (here, 25°C).

[0005] Patent Documents 1 and 2 propose methods for improving storage stability using certain specific phosphite ester compounds. While these methods dramatically improve storage stability, they have problems such as the inability to obtain a sufficiently cured organopolysiloxane cured product without exposure to high temperatures of around 150°C, the susceptibility of phosphite ester compounds to hydrolysis and poor storage stability in air, and the tendency of the catalyst to recrystallize when the coordination number of the phosphite ester compound is high. Therefore, there has been a demand for a platinum-phosphite ester complex-containing hydrosilylation catalyst that is organic solvent-free and liquid at 23°C. Obtaining such a catalyst would enable the production of curable organopolysiloxane compositions that are organic solvent-free and have stable properties and physical properties. Therefore, there has been a growing demand for a platinum-phosphite ester complex-containing hydrosilylation catalyst that is organic solvent-free and liquid at 23°C.

[0006] International Publication No. 2021 / 014970 Japanese Patent Application Laid-Open No. 2021-042323

[0007] The present invention has been made to solve these problems, and its object is to obtain a platinum-phosphite complex-containing hydrosilylation catalyst that is liquid at 23°C even without containing an organic solvent, thereby improving the stability of the catalyst's properties, and to obtain an organic solvent-free curable silicone composition by using this catalyst in a curable organopolysiloxane composition. Another object of the present invention is to provide an organopolysiloxane composition whose properties and physical characteristics are stable even when exposed to temperatures above room temperature for long periods of time.

[0008] In order to achieve the above object, the present invention is the result of extensive research and provides a hydrosilylation catalyst containing a platinum-phosphite complex formed by association of a platinum-phosphite complex with a silane compound and / or a partial hydrolyzate thereof.

[0009] That is, the present invention provides a platinum-phosphite complex-containing hydrosilylation catalyst, which is an association of the following components (A) and (B), which is free of organic solvents and is liquid at 23° C.: (A) a platinum-phosphite complex composed of platinum and a phosphite compound represented by the following general formula (1): (In the formula, R 1 is a hydrogen atom or a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms; and (B) a silane compound represented by the following general formula (2) and / or a partial hydrolyzate thereof: (In the formula, R 2 represents an alkenyl group having 2 to 10 carbon atoms, and R 3 is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms. X is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms or OR 3 is)

[0010] The component (B) is 2 is preferably an alkoxysilane derivative in which the group is a vinyl group.

[0011] The platinum-phosphite complex-containing hydrosilylation catalyst obtained by associating a complex of a phosphite compound represented by formula (1) with a silane compound represented by formula (2) and / or a partial hydrolyzate thereof can be maintained in a liquid state at room temperature. This provides the advantages of good workability when blending the catalyst into a curable organopolysiloxane composition, as well as facilitating uniform dispersion.

[0012] The present invention can provide an organic solvent-free curable organopolysiloxane composition that contains the platinum-phosphite complex-containing hydrosilylation catalyst described above.

[0013] Such a curable organopolysiloxane composition remains stable in properties and physical characteristics even when exposed to temperatures above room temperature for extended periods of time, and it is possible to provide articles comprising a cured product of the composition.

[0014] The present invention also provides a method for producing the platinum-phosphite complex-containing hydrosilylation catalyst composition, comprising the following steps (a) to (d): (a) preparing a solution of a phosphite compound represented by the following general formula (1) in a hydrocarbon solvent having a boiling point of 80°C or lower; (In the formula, R1 is a hydrogen atom or a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms.) (b) adding an organic solvent-free platinum compound selected from the group consisting of platinum chloride, chloroplatinic acid, or complexes of chloroplatinic salts with vinyl group-containing siloxanes to the solution, and dispersing the compound to prepare a solution containing a platinum-phosphite complex; (c) adding a silane compound represented by the following general formula (2) and / or a partial hydrolyzate thereof to the solution obtained by steps (a) and (b), and dispersing the compound to prepare a solution containing an association product of at least a portion of the platinum-phosphite complex and the silane compound represented by the following general formula (2) and / or a partial hydrolyzate thereof; (In the formula, R 2 represents an alkenyl group having 2 to 10 carbon atoms, and R 3 is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms. X is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms or OR 3 (d) a step of removing the hydrocarbon solvent from the solution obtained in the step (c).

[0015] By carrying out the steps (a) to (d), a platinum-phosphite complex-containing hydrosilylation catalyst can be produced stably.

[0016] In step (c), the molar ratio of alkenyl groups in the silane compound represented by general formula (2) and / or its partial hydrolysate to one platinum atom in the platinum compound is preferably within the range of 0.01 to 500. A ratio of 0.01 or more allows the catalyst to maintain a liquid state at 23°C, and prevents crystal precipitation, which can lead to problems such as poor dispersibility and reduced compounding workability in curable organopolysiloxane compositions containing the catalyst. A ratio of 500 or less prevents the amount of silane compound represented by general formula (2) and / or its partial hydrolysate from being added from being too large, resulting in an appropriate molecular weight for the siloxane compound itself, no adverse effect on the viscosity of the resulting platinum-phosphite complex-containing hydrosilylation catalyst, good property stability for the resulting platinum-phosphite complex-containing hydrosilylation catalyst, and favorable workability when compounding the catalyst.

[0017] The platinum-phosphite complex-containing hydrosilylation catalyst of the present invention is liquid at 23°C even without the addition of an organic solvent, and therefore exhibits excellent stability in the properties of the catalyst itself. Furthermore, when the catalyst is incorporated into a curable silicone composition, it can be easily dispersed uniformly, resulting in an organic solvent-free curable organopolysiloxane composition. The resulting organic solvent-free curable organopolysiloxane composition provides an organopolysiloxane composition that exhibits stable properties and physical characteristics even when exposed to temperatures above room temperature for extended periods of time. Furthermore, because it does not contain organic solvents, it is possible to obtain an extremely safe organopolysiloxane cured product.

[0018] The present inventors have searched for catalysts useful as resin curing catalysts, particularly as curing catalysts for organopolysiloxane compositions, and have found that an association product of platinum and a platinum-phosphite ester complex represented by the following general formula (1) with a silane compound represented by the following general formula (2) and / or a partial hydrolyzate thereof is useful, leading to the completion of the present invention, including a method for producing the same.

[0019] That is, the present invention provides a compound represented by the following general formula (1): (In the formula, R 1 (B) a silane compound represented by the following general formula (2) and / or a partial hydrolyzate thereof; (In the formula, R 2 represents an alkenyl group having 2 to 10 carbon atoms, and R 3 is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms. X is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms or OR 3 The hydrosilylation catalyst is a platinum-phosphite complex-containing hydrosilylation catalyst that is an association of the component (A) and the component (B), does not contain an organic solvent, and is liquid at 23°C.

[0020] The present invention also provides a method for producing a platinum-phosphite complex-containing hydrosilylation catalyst, comprising the following steps (a) to (d): (a) preparing a solution of a phosphite compound represented by the following general formula (1) in a hydrocarbon solvent having a boiling point of 80° C. or lower; (In the formula, R 1 is a hydrogen atom or a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms.) (b) adding an organic solvent-free platinum compound selected from the group consisting of platinum chloride, chloroplatinic acid, or a complex of a chloroplatinate with a vinyl group-containing siloxane to the solution and dispersing the compound to prepare a solution containing a platinum-phosphite complex; (c) adding a silane compound represented by the following general formula (2) and / or a partial hydrolyzate thereof to the solution obtained in steps (a) and (b) above and dispersing the compound to prepare a solution containing an association product of at least a portion of the platinum-phosphite complex and the silane compound represented by the following general formula (2) and / or a partial hydrolyzate thereof; (In the formula, R 2 represents an alkenyl group having 2 to 10 carbon atoms, and R 3 is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms. X is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms or OR 3 (d) a step of removing the hydrocarbon solvent from the solution obtained in the step (c).

[0021] [Phosphite Compound] The phosphite compound used in the present invention, represented by the following general formula (1), forms a complex with platinum, and is an essential component for dramatically improving the storage stability of the properties and physical characteristics of the curable organopolysiloxane composition containing a platinum-phosphite complex-containing hydrosilylation catalyst obtained using this compound. (In the formula, R 1 is a hydrogen atom or a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms.

[0022] In the above general formula (1), R 1are independently a hydrogen atom or a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms, preferably 1 to 2 carbon atoms, more preferably 1 carbon atom, i.e., a methyl group. Specific examples of the phosphite ester compound include R phosphates such as tris(2,4-dimethylphenyl)phosphite, tris(2,4-di-tert-butylphenyl)phosphite, tris(2,4-bis(3-ethylpentan-3-yl)phenyl)phosphite, and tris(2,4-bis(4-propylheptan-4-yl)phenyl)phosphite. 1 and phosphite compounds having the same number of carbon atoms, and compounds having R such as tris(4-(tert-butyl)-2-methylphenyl)phosphite, tris(4-(tert-butyl)-2-ethylphenyl)phosphite, tris(2-(tert-butyl)-4-(3-ethylpentan-3-yl)phenyl)phosphite, and tris(2-(tert-butyl)-4-(3-methylhexan-3-yl)phenyl)phosphite. 1 Among these, it is particularly preferable to use tris(2,4-di-tert-butylphenyl)phosphite, which is easily available and has excellent storage stability.

[0023] The optimal amount of the phosphite compound used in the present invention is greater than 0.6 molecules and not more than 3.0 molecules per platinum molecule, and more preferably, it is added in an amount of 0.8 to 2.5 molecules per platinum molecule. Here, when the amount exceeds 0.6 molecules per platinum molecule, the storage stability of the curable organopolysiloxane composition containing the catalyst is good, and the risk of gelation of the organopolysiloxane composition is eliminated. On the other hand, when the amount is 3.0 molecules or less per platinum molecule, even when the catalyst is associated with a silane compound and / or a partial hydrolyzate thereof, as described below, there is no risk of crystal precipitation at room temperature, and the platinum-phosphite complex-containing hydrosilylation catalyst can be sufficiently maintained in a liquid state. Furthermore, the catalyst exhibits good dispersibility in the curable organopolysiloxane composition containing the catalyst, and problems such as reduced compounding workability are avoided.

[0024] [Silane Compound and / or Partial Hydrolyzate thereof] The silane compound and / or partial hydrolyzate thereof represented by the following general formula (2) is used in the present invention. (In the formula, R 2 represents an alkenyl group having 2 to 10 carbon atoms, and R 3 is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms. X is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms or OR 3 The silane compound represented by the formula (I) and / or its partial hydrolyzate is an essential component for associating with the complex of platinum and a phosphite compound and preventing crystallization at room temperature.

[0025] In the above general formula (2), R 2 is an alkenyl group having 2 to 10 carbon atoms, preferably 2 to 10 carbon atoms, more preferably 2 to 8 carbon atoms, and most preferably a vinyl group. 3 is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms. Specific examples include a methyl group, an ethyl group, a propyl group, an isopropyl group, a 3-propenyl group, and an isopropenyl group. A group having 1 or 2 carbon atoms is preferred, and a group having 1 carbon atom, i.e., a methyl group, is more preferred. Specific examples of siloxane compounds include vinyl group-containing alkoxysilanes such as vinyltrimethoxysilane, vinyldimethoxymethylsilane, vinyltriethoxysilane, vinyldiethoxymethylsilane, allyltrimethoxysilane, allyldimethoxymethylsilane, 7-octenyltrimethoxysilane, and 7-octenyldimethoxymethylsilane, and / or partial hydrolysates thereof. In the above general formula (2), X is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms or OR 3 Specific examples include a methyl group, an ethyl group, a propyl group, a methoxy group, an ethoxy group, a propoxy group, and an isopropoxy group.

[0026] The optimal amount of the silane compound and / or its partial hydrolyzate used in the present invention is 0.05 mol % or more and 100 mol % or less per platinum molecule, and more preferably 0.05 mol % or more and 90 mol % or less per platinum molecule. When the amount is 0.05 mol % or more per platinum molecule, the resulting platinum-phosphite complex-containing hydrosilylation catalyst does not crystallize at room temperature, can maintain its liquid state, and exhibits good dispersibility in curable organopolysiloxane compositions containing the catalyst, preventing problems such as reduced compounding workability. Furthermore, if the amount is 100 mol % or less per platinum molecule, the platinum-phosphite complex-containing hydrosilylation catalyst itself will be stable, and the effective platinum amount of the platinum-phosphite complex-containing hydrosilylation catalyst itself will not decrease. Therefore, when a curable organopolysiloxane composition containing the catalyst is obtained, the amount blended will be appropriate, and the amount of the silane compound and / or its partial hydrolyzate added will also be appropriate, resulting in good mechanical properties and curability.

[0027] One of the features of the platinum-phosphite complex-containing hydrosilylation catalyst of the present invention is that it does not contain a hydrocarbon organic solvent. Here, "hydrocarbon organic solvent" refers to an aliphatic hydrocarbon solvent or an aromatic hydrocarbon solvent. Aliphatic hydrocarbon solvents include not only hydrocarbon solvents with a boiling point of 80°C or less that are used in step (a) of the catalyst production method described below, but also aliphatic hydrocarbon solvents with a boiling point above 80°C. Specific examples include n-pentane, n-hexane, 2-methylbutane, 2,2-dimethylbutane, 2,3-dimethylbutane, 2-methylpentane, 3-methylpentane, n-heptane, and n-octane. Examples of aromatic hydrocarbons include benzene, toluene, xylene, ethylbenzene, and isopropylbenzene.

[0028] [Use of Platinum-Phosphite Complex-Containing Hydrosilylation Catalyst] The platinum-phosphite complex-containing hydrosilylation catalyst described above can be used in applications such as curing catalysts for various resins and purification catalysts. However, its unique characteristics are particularly apparent when used as a curing catalyst for organopolysiloxane compositions that undergo a hydrosilylation reaction to produce a resin (or gel). This is because, upon heating, it exhibits curability nearly equivalent to that of conventional platinum compound-based hydrosilylation catalysts, and, upon storage at room temperature, the phosphite compound forms a complex with platinum, suppressing catalytic activity and significantly slowing the progress of the hydrosilylation reaction. Therefore, curable organopolysiloxane compositions using this catalyst exhibit stable properties and physical characteristics even when exposed to temperatures above room temperature for extended periods. Furthermore, by associating a complex of a phosphite compound and platinum with a silane compound represented by general formula (2) and / or a partial hydrolyzate thereof, the resulting platinum-phosphite complex-containing hydrosilylation catalyst can be maintained in a liquid state at room temperature. This has the advantage that the catalyst is easy to work with when blended into a curable organopolysiloxane composition, and that it is easily dispersed uniformly.

[0029] The amount of platinum-phosphite complex-containing hydrosilylation catalyst blended into the curable organopolysiloxane composition is 0.001 to 10.0 parts by mass, preferably 0.010 to 5.0 parts by mass, and more preferably 0.050 to 3.0 parts by mass per 100 parts by mass of the alkenyl group-containing polymer. When the amount of platinum-phosphite complex-containing hydrosilylation catalyst is 0.001 part by mass or more, the resulting silicone rubber composition has sufficient strength and is free from poor curing. Conversely, when the amount of platinum-phosphite complex-containing hydrosilylation catalyst blended is 10.0 parts by mass or less, the resulting silicone rubber composition does not become discolored or require a short curing time, and is also cost-effective. The activity of the catalyst, i.e., the curability, can be controlled by increasing or decreasing the concentration of the platinum-phosphite complex-containing hydrosilylation catalyst added.

[0030] [Method for producing a platinum-phosphite complex-containing hydrosilylation catalyst] [Step (a)] Step (a) is a step of preparing a solution by dissolving a phosphite compound represented by general formula (1) in a hydrocarbon solvent having a boiling point of 80°C or lower. (In the formula, R 1 is a hydrogen atom or a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms.

[0031] If the phosphite ester compound is liquid at room temperature, a complex can be easily formed in step (b) below by blending it with an organic solvent-free platinum compound selected from the group consisting of complexes of platinum chloride, chloroplatinic acid, or chloroplatinate salts with vinyl group-containing siloxanes. However, since many of the phosphite ester compounds are solid at room temperature, it is possible to dissolve the phosphite ester compound in a hydrocarbon solvent in step (a) above and then blend it with an organic solvent-free platinum compound selected from the group consisting of complexes of platinum chloride, chloroplatinic acid, or chloroplatinate salts with vinyl group-containing siloxanes to rapidly form a complex.

[0032] The hydrocarbon solvent having a boiling point of 80°C or lower may be linear or branched. Specific examples of hydrocarbon solvents having a boiling point of 80°C or lower include n-pentane (boiling point: 36°C), n-hexane (boiling point: 68°C), 2-methylbutane (boiling point: 30°C), 2,2-dimethylbutane (boiling point: 50°C), 2,3-dimethylbutane (boiling point: 58°C), 2-methylpentane (boiling point: 62°C), and 3-methylpentane (boiling point: 63°C). Among these, n-hexane (boiling point: 68°C) is particularly suitable for industrial use because it is relatively easy to handle and easily removed in the subsequent removal step. From the viewpoint of vacuum distillation of the hydrocarbon solvent, it is preferable that the boiling point of the hydrocarbon solvent used be 80°C or lower. While the lower limit is not particularly limited, it is preferably about 0°C or higher. In this case, by setting the vacuum distillation temperature to 40°C or lower, a stable platinum-phosphite complex-containing hydrosilylation catalyst can be obtained. In the case of hydrocarbon solvents with a boiling point of 80°C or higher, the used hydrocarbon solvent cannot be completely removed unless the reduced-pressure distillation temperature is 40°C or higher. This may result in the hydrocarbon solvent remaining in the platinum-phosphite complex-containing hydrosilylation catalyst, or in the platinum-phosphite complex-containing hydrosilylation catalyst being decomposed by the temperature in the solvent removal step, resulting in the precipitation of crystals.

[0033] There are no particular restrictions on the amount of hydrocarbon solvent used that has a boiling point of 80°C or lower. The temperature at which the phosphite ester compound represented by general formula (1) is dissolved in the hydrocarbon solvent is 40°C or lower, more preferably in the range of 0 to 35°C. Dissolution at 40°C or lower makes the phosphite ester compound represented by general formula (1) less susceptible to hydrolysis with the water contained in the hydrocarbon solvent. This prevents the phosphite ester compound represented by formula (1) from converting to a phosphate ester compound, resulting in a stable platinum-phosphite complex-containing hydrosilylation catalyst. There are no particular restrictions on the dissolution time. It is preferable to select a container that can block oxygen for dissolution.

[0034] [Step (b)] Step (b) is a step of adding an organic solvent-free platinum compound selected from the group consisting of platinum chloride, chloroplatinic acid, or a complex of a chloroplatinate with a vinyl group-containing siloxane to the solution and dispersing the compound to prepare a solution containing a platinum-phosphite complex.

[0035] [Organic Solvent-Free Platinum Compound Selected from the Group Consisting of Platinum Chloride, Chloroplatinic Acid, or Complexes of Chloroplatinic Salts with Vinyl Group-Containing Siloxanes] The organic solvent-free platinum compound used in the present invention, selected from the group consisting of platinum chloride, chloroplatinic acid, or complexes of chloroplatinic salts with vinyl group-containing siloxanes, is usually a curing catalyst that promotes the hydrosilylation addition reaction of SiH groups in an organohydrogenpolysiloxane to an alkenyl group-containing polymer contained in a curable organopolysiloxane composition. In the present invention, a phosphite ester compound represented by general formula (1), (In the formula, R 1 is a hydrogen atom or a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms.) By forming a complex with the silane compound represented by general formula (2) and / or a partial hydrolyzate thereof, the properties and storage stability of the curable organopolysiloxane composition obtained using the complex can be significantly improved. (In the formula, R 2 represents an alkenyl group having 2 to 10 carbon atoms, and R 3 is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms. X is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms or OR 3 By associating this catalyst with a platinum-phosphite complex, a platinum-phosphite complex-containing hydrosilylation catalyst can be obtained that is liquid at room temperature without the need for an organic solvent. This improves the uniform dispersion of the catalyst when a curable organopolysiloxane composition is obtained using this catalyst, as well as the stability and uniformity of the catalyst's properties.

[0036] Specific examples of organic solvent-free platinum compounds selected from the group consisting of platinum chloride, chloroplatinic acid, or complexes of chloroplatinic salts with vinyl group-containing siloxanes include platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (Karstedt complex), platinum-1,3-diallyl-1,1,3,3-tetramethyldisiloxane complex, platinum-1,3-divinyl-1,3-dimethyl-1,3-diphenyldisiloxane complex, platinum-1,1,3,3-tetraphenyldisiloxane complex, and platinum-1,3,5,7-tetramethyl-1,3,5,7-tetravinylcyclotetrasiloxane complex. It is essential that the compound contains at least one hydrosilylation catalyst selected from this group, and that the compound does not contain an organic solvent. Among the above-mentioned organic solvent-free hydrosilylation catalysts, it is particularly preferred to use a platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (Karstedt complex).

[0037] The organic solvent-free platinum compound selected from the group consisting of platinum chloride, chloroplatinic acid, or a complex of a chloroplatinate with a vinyl group-containing siloxane, as shown here, must be free of basic organic solvents such as aromatic hydrocarbon organic solvents such as toluene and xylene, and alcohol organic solvents such as ethanol, n-butanol, and 2-ethylhexyl alcohol (excluding low-molecular-weight vinyl group-containing siloxanes such as tetramethyldivinylsiloxane, trimethyltrivinylcyclotrisiloxane, and tetramethyltetravinylcyclotetrasiloxane).

[0038] The organic solvent-free platinum compound selected from the group consisting of platinum chloride, chloroplatinic acid, or complexes of chloroplatinic salts with vinyl-containing siloxanes is typically used in the form of a solution in a siloxane that forms the ligand of the platinum-siloxane complex. The solution is typically prepared so that the platinum atom content is approximately 0.001 to 0.010 moles. This is to enhance the stability of the platinum-siloxane complex. The mass percent of platinum contained is 0.2 to 2.0%. Examples of compounds that can form platinum-siloxane complexes are tetramethyldivinylsiloxane, trimethyltrivinylcyclotrisiloxane, and tetramethyltetravinylcyclotetrasiloxane.

[0039] A preferred platinum compound is platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (Karstedt complex), which is believed to have the following structure: The time required for this step is preferably 30 minutes or more at a temperature of 40° C. or less. As in step (a), it is preferable to select a container for step (b) that can block oxygen.

[0040] [Step (c)] Step (c) is a step of adding a silane compound represented by the following general formula (2) and / or a partial hydrolysate thereof to the solution obtained in steps (a) and (b) and dispersing the compound to prepare a solution containing an association product of at least a portion of the platinum-phosphite ester complex and the silane compound represented by the following general formula (2) and / or a partial hydrolysate thereof: (In the formula, R 2 represents an alkenyl group having 2 to 10 carbon atoms, and R 3 is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms. X is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms or OR 3 is)

[0041] This step is preferably carried out at a temperature of 40°C or less for 60 minutes or more. As with step (a), it is preferable to select a container that can block oxygen for this step. The silane compound represented by general formula (2) and / or its partial hydrolyzate used here is selected from the group consisting of platinum chloride, chloroplatinic acid, or a complex of a chloroplatinate salt with a vinyl group-containing siloxane, and is formed by mixing 1 platinum atom of the silane compound represented by general formula (2) with 1 platinum atom of the platinum compound containing no organic solvent. 2 It is preferable to add the silane compound in an amount such that the unit is in the range of 0.01 to 500 times. 2 When the ratio of the units represented by the units is 0.01 times or more, the amount of the silane compound represented by general formula (2) and / or its partial hydrolyzate added per platinum atom is sufficient, and the catalyst can be reliably maintained in a liquid state at 23°C, and problems such as poor dispersibility and poor blending workability in the curable organopolysiloxane composition containing the catalyst due to precipitation of crystals do not occur. 2 When the ratio of the units is 500 times or less, the amount of the silane compound represented by general formula (2) and / or its partial hydrolyzate added is appropriate, and the molecular weight of the siloxane compound itself becomes large, which does not significantly affect the viscosity of the resulting platinum-phosphite complex-containing hydrosilylation catalyst, does not deteriorate the stability of the properties of the resulting platinum-phosphite complex-containing hydrosilylation catalyst, and does not result in problems such as reduced workability when compounding the catalyst.

[0042] [Step (d)] Step (d) is a step of removing the hydrocarbon solvent from the solution obtained in steps (a) to (c) above. This step is essential for removing the hydrocarbon solvent from the solution obtained in steps (a) to (c) and obtaining a platinum-phosphite complex-containing hydrosilylation catalyst free of organic solvents. The solvent removal method used here is preferably a reduced-pressure distillation method in which the solvent is distilled off under reduced pressure using a vacuum pump or the like. This is because a stable platinum-phosphite complex-containing hydrosilylation catalyst can be obtained by setting the reduced-pressure distillation temperature to 40°C or less. The degree of vacuum varies depending on the boiling point of the hydrocarbon solvent used, but by setting the pressure to 50 hPa or less, the hydrocarbon solvent used can be completely removed. Whether the hydrocarbon solvent used has been completely removed can be confirmed by measuring the weight ratio of the total weight of the phosphite compound, platinum compound, and silane compound used to the platinum-phosphite complex-containing hydrosilylation catalyst obtained after completion of step (d). If the weight of the resulting platinum-phosphite complex-containing hydrosilylation catalyst is greater than the total weight of the phosphite compound, platinum compound, and silane compound used, the hydrocarbon solvent will remain, and the hydrocarbon solvent can be completely removed by adding an additional time to the present step.

[0043] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited thereto. In the examples, "parts" means "parts by mass" and "%" means "% by mass".

[0044] Example 1: 0.6622 parts of tris(2,4-di-tert-butylphenyl)phosphite was weighed into a 25 g transparent glass container, and 9.3378 parts of n-hexane was added. The container was sealed and allowed to dissolve at room temperature for approximately 1 hour. After visually confirming that the tris(2,4-di-tert-butylphenyl)phosphite crystals had dissolved, 10.0 parts of a platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex containing 1% Pt atoms was added, the container was sealed, and the mixture was stirred for 30 minutes to achieve uniformity. Thereafter, 0.06 parts of vinyltrimethoxysilane was added, the container was sealed, and the mixture was stirred for 60 minutes to achieve uniformity. The solution was then transferred to a 100 ml eggplant-shaped flask, and the n-hexane was distilled off under reduced pressure using a rotary evaporator (conditions: 30°C x 2 hours / approximately 35 hPa). A 100 ml recovery flask yielded 10.31 g of a colorless, transparent liquid (yield: 96.2%). This platinum-phosphite complex-containing hydrosilylation catalyst was designated "Catalyst 1." (The amount of phosphite compound blended was 2.0 molecules per platinum molecule in the platinum compound, and the amount of silane compound blended was 0.79 molecules per platinum molecule in the platinum compound.)

[0045] Example 2: 0.3311 parts of tris(2,4-di-tert-butylphenyl)phosphite was weighed into a 25 g transparent glass container, and 9.6689 parts of n-hexane was added. The container was sealed and allowed to dissolve at room temperature for approximately 1 hour. After visually confirming that the tris(2,4-di-tert-butylphenyl)phosphite crystals had dissolved, 10.0 parts of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex containing 1% Pt atoms was added, the container was sealed, and the mixture was stirred for 30 minutes to achieve uniformity. Thereafter, 0.06 parts of vinyltrimethoxysilane was added, the container was sealed, and the mixture was stirred for 60 minutes to achieve uniformity. The solution was then transferred to a 100 ml eggplant-shaped flask, and the n-hexane was distilled off under reduced pressure using a rotary evaporator (conditions: 30°C x 2 hours / approximately 32 hPa). A 100 ml recovery flask yielded 10.25 g of a colorless, transparent liquid (yield: 98.7%). This platinum-phosphite complex-containing hydrosilylation catalyst was designated "Catalyst 2." (The amount of phosphite compound blended was 1.0 molecule per platinum molecule in the platinum compound, and the amount of silane compound blended was 0.79 molecule per platinum molecule in the platinum compound.)

[0046] Example 3: 0.3311 parts of tris(2,4-di-tert-butylphenyl)phosphite was weighed into a 25 g transparent glass container, and 9.6689 parts of n-hexane was added. The container was sealed and allowed to dissolve at room temperature for approximately 1 hour. After visually confirming that the tris(2,4-di-tert-butylphenyl)phosphite crystals had dissolved, 10.0 parts of a platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex containing 1% Pt atoms was added, the container was sealed, and the mixture was stirred for 30 minutes to achieve uniformity. Thereafter, 1.00 parts of vinyltrimethoxysilane was added, the container was sealed, and the mixture was stirred for 60 minutes to achieve uniformity. The solution was then transferred to a 100 ml eggplant-shaped flask, and the n-hexane was distilled off under reduced pressure using a rotary evaporator (conditions: 30°C x 2 hours / approximately 34 hPa). A 100 ml recovery flask yielded 11.12 g of a colorless, transparent liquid (yield: 98.1%). This platinum-phosphite complex-containing hydrosilylation catalyst was designated "Catalyst 3." (The amount of phosphite compound blended was 1.0 molecule per platinum molecule in the platinum compound, and the amount of silane compound blended was 13.16 molecules per platinum molecule in the platinum compound.)

[0047] Example 4: 0.6622 parts of tris(2,4-di-tert-butylphenyl)phosphite was weighed into a 25 g transparent glass container, and 9.3378 parts of n-hexane was added. The container was sealed and allowed to dissolve at room temperature for approximately 1 hour. After visually confirming that the tris(2,4-di-tert-butylphenyl)phosphite crystals had dissolved, 10.0 parts of a platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex containing 1% Pt atoms was added, the container was sealed, and the mixture was stirred for 30 minutes to achieve uniformity. Thereafter, 0.06 parts of 7-octenyltrimethoxysilane (product name: KBM-1083 [manufactured by Shin-Etsu Chemical Co., Ltd.]) was added, the container was sealed, and the mixture was stirred for 60 minutes to achieve uniformity. The solution was then transferred to a 100 ml recovery flask, and n-hexane was distilled off under reduced pressure using a rotary evaporator (conditions: 30°C x 2 hours / approximately 35 hPa). 10.31 g of a colorless, transparent liquid was obtained in the 100 ml recovery flask (yield: 96.2%). This platinum-phosphite complex-containing hydrosilylation catalyst was designated "Catalyst 4." (The amount of phosphite compound blended was 2.0 molecules per platinum molecule in the platinum compound, and the amount of silane compound blended was 0.50 molecules per platinum molecule in the platinum compound.)

[0048] Comparative Example 1 The same procedure as in Example 1 was carried out, except that 0.06 parts of 2,4,6,8-tetravinyl-2,4,6,8-tetramethylcyclotetrasiloxane was used instead of vinyltrimethoxysilane. As a result, 10.33 g of a colorless, transparent liquid was obtained in a 100 ml eggplant-shaped flask (yield: 96.3%). This platinum-phosphite complex-containing hydrosilylation catalyst is designated "Catalyst 5." (The amount of phosphite compound blended was 1.0 molecule per platinum molecule in the platinum compound, and the amount of silane compound blended was 0 molecule per platinum molecule in the platinum compound. [The amount of 2,4,6,8-tetravinyl-2,4,6,8-tetramethylcyclotetrasiloxane, the ligand, blended was 0.34 molecules per platinum molecule in the platinum compound.])

[0049] Comparative Example 2 The same procedure as in Example 1 was carried out, except that vinyltrimethoxysilane was omitted. As a result, 10.50 g of a colorless, transparent liquid was obtained in a 100 ml eggplant-shaped flask (yield: 98.5%). This platinum-phosphite complex-containing hydrosilylation catalyst is designated "Catalyst 6." (The amount of phosphite compound blended was 1.0 molecule per platinum molecule in the platinum compound, and the amount of silane compound blended was 0 molecule per platinum molecule in the platinum compound.)

[0050] [Comparative Example 3] 0.3311 parts of tris(2,4-di-tert-butylphenyl)phosphite was weighed into a 25 g transparent glass container, and 9.6689 parts of n-heptane (boiling point: 98 ° C) was added. After sealing, the container was allowed to dissolve at room temperature for approximately 1 hour. After visually confirming that the tris(2,4-di-tert-butylphenyl)phosphite crystals had dissolved, 10.0 parts of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex having 1% Pt atoms was added, the container was sealed, and the mixture was stirred for 30 minutes to become uniform. Thereafter, 0.06 parts of vinyltrimethoxysilane was added, the container was sealed, and the mixture was stirred for 60 minutes to become uniform. Thereafter, the solution was transferred to a 100 ml eggplant-shaped flask, and n-hexane was distilled off under reduced pressure using a rotary evaporator (conditions: 50 ° C × 2 hours / approximately 35 hPa). A 100 ml eggplant-shaped flask was filled with a colorless, transparent liquid (yield: 10.95 g) containing dispersed white crystals; a colorless, transparent liquid was not obtained (yield: 105.4%). This platinum-phosphite complex-containing hydrosilylation catalyst is designated "Catalyst 7." (The amount of phosphite compound blended was 1.0 molecule per platinum molecule in the platinum compound, and the amount of silane compound blended was 0.79 molecule per platinum molecule in the platinum compound.)

[0051] Comparative Example 4: The same procedure as in Example 1 was carried out, but without using n-hexane. As a result, a liquid containing dispersed white crystals (yield: 10.33 g) was obtained in a 100 ml eggplant-shaped flask; a colorless, transparent liquid could not be obtained (yield: 99.9%). This platinum-phosphite complex-containing hydrosilylation catalyst was designated "Catalyst 8."

[0052] The yields and yields of the platinum-phosphite complex-containing hydrosilylation catalysts obtained in Examples 1 to 4 and Comparative Examples 1 to 4 are shown in Table 1. The catalysts obtained in these Examples and Comparative Examples were also subjected to the following test for their appearance. The resulting platinum-phosphite complex-containing hydrosilylation catalysts were stored in sealed containers filled with nitrogen. The appearance was then checked after 7 days at 23°C, and catalysts that showed no formation of crystals in the container were rated as passing, while catalysts that showed formation of crystals were rated as failing. The results are shown in Table 1.

[0053]

[0054] [Evaluation] The platinum-phosphite ester complex-containing hydrosilylation catalysts obtained in Examples 1 to 4 satisfy the requirements of the present invention. In all Examples, the amount of phosphite ester compound was 1.0 or 2.0 molecules per platinum molecule of the platinum compound. However, the same procedure was repeated to increase the amount of phosphite ester compound per platinum molecule of the platinum compound in increments of 0.1 molecules up to 3.0 molecules. It was confirmed that a colorless, transparent liquid was obtained in all cases. The platinum-phosphite ester complex-containing hydrosilylation catalysts obtained in Examples 1 to 4 exhibited suppressed crystal precipitation even after being left at 23°C for 7 days under sealed conditions, demonstrating that platinum-phosphite ester complex-containing hydrosilylation catalysts with highly stable properties were obtained. In contrast, the platinum-phosphite ester complex-containing hydrosilylation catalysts of Comparative Examples 1 and 2, which lack the addition of the silane compound represented by general formula (2) and / or its partial hydrolysate, exhibit crystal precipitation after approximately 7 days at 23°C. Furthermore, the platinum-phosphite ester complex-containing hydrosilylation catalyst of Comparative Example 3 uses n-heptane, which has a boiling point of 80°C or higher, as the hydrocarbon solvent for dissolving the phosphite ester compound. Therefore, even when the temperature for vacuum distillation was increased, the n-heptane used could not be completely distilled off. Furthermore, increasing the heating temperature resulted in the phosphite ester compound in the platinum-phosphite ester complex-containing hydrosilylation catalyst becoming discoordinated, resulting in the precipitation of crystals, making it impossible to obtain a liquid platinum-phosphite ester complex-containing hydrosilylation catalyst. The platinum-phosphite ester complex-containing hydrosilylation catalyst of Comparative Example 4 coordinated the phosphite ester compound to the platinum compound without dissolving it in a hydrocarbon solvent. As a result, the phosphite ester compound did not dissolve, resulting in a liquid in which the crystals were dispersed. These results confirm the effectiveness of the catalyst production method of the present invention for obtaining a stable liquid platinum-phosphite ester complex-containing hydrosilylation catalyst.

[0055] [Examples of Curable Organopolysiloxane Compositions Utilizing Platinum-Phosphite Complex-Containing Hydrosilylation Catalysts] Examples and comparative examples relating to curable organopolysiloxane compositions utilizing the platinum-phosphite complex-containing hydrosilylation catalysts obtained according to the present invention will now be described in detail. Note that the following examples and comparative examples are of one-component millable silicone rubber compositions, but the present invention is not limited thereto.

[0056] The evaluation of this example was carried out as follows.

[0057] [Regarding workability in preparing one-component millable silicone rubber compositions] When preparing the one-component millable silicone rubber compositions prepared in the following examples and comparative examples, those in which the platinum-phosphite complex-containing hydrosilylation catalyst was liquid and no problems occurred when it was added were judged to pass. Conversely, those in which the platinum-phosphite complex-containing hydrosilylation catalyst crystallized during catalyst blending and problems occurred in workability when it was added were judged to fail.

[0058] [Storage Stability of One-Component Millable Silicone Rubber Compositions] The storage stability of the one-component millable silicone rubber compositions prepared in the following examples and comparative examples was evaluated by comparing the initial curing properties of the resulting one-component millable silicone rubber compositions with the curing properties after 6 months of storage at 23°C using a rheometer (RUBBER PROCESS ANALYZER RPA2000, manufactured by ALPHA TECHNOLOGIES). Those that could be evaluated after 6 months at 23°C were judged to pass. Here, the curing data for the one-component millable silicone rubber compositions are shown as measurements taken at 150°C. In Table 2, T50* and T50** represent the time T from when the torque stabilizes on the time-torque curve at 150°C, assuming that 100% curing has occurred, and T50 represents the time T from when the torque rises to when it reaches 50%.

[0059] Composition Example 1: 100 parts by mass of organopolysiloxane gum having an average degree of polymerization of 6,000 and consisting of 99.85 mol % dimethylsiloxane units, 0.125 mol % methylvinylsiloxane units, and 0.025 mol % dimethylvinylsiloxy units, and a BET specific surface area of ​​200 m 2 55 parts by mass of fumed silica (Aerosil 200, manufactured by Nippon Aerosil Co., Ltd.) with a molecular weight of 1 / g, 12 parts by mass of dimethyldimethoxysilane, 0.2 parts by mass of vinyltrimethoxysilane, 12 parts by mass of dimethylpolysiloxane having silanol groups at both ends, an average degree of polymerization of 4, and a viscosity at 25°C of 15 mPa·s, and 0.15 parts by mass of 3% potassium siliconate were added, and the mixture was heated at 170°C for 2 hours while mixing in a kneader to prepare base compound (1). A mixture of 100 parts by mass of organopolysiloxane raw rubber and 50 parts by mass of a rubber having a set structure of M was added to base compound (1). 2 D H 20 D 18 (H amount: 0.00726 mol / g) (wherein M: (CH 3 ) 3 SiO 1/2 -, D H :(CH 3 ) HSiO 2/2 -, D: (CH 3 ) 2 SiO 2/2 1.7 parts by mass of organohydrogensiloxane (representing -), and 0.05 parts by mass of "Catalyst 1" prepared in Example 1 were added and mixed uniformly using a twin roll mill to produce a one-component silicone rubber composition 1 in a raw rubber state.

[0060] Composition Example 2 One-component silicone rubber composition 2 was prepared in the same manner as in Composition Example 1, except that 0.05 parts by mass of "catalyst 2" was used in place of "catalyst 1."

[0061] Composition Example 3 One-component silicone rubber composition 3 was prepared in the same manner as in Composition Example 1, except that 0.05 parts by mass of "catalyst 3" was used in place of "catalyst 1."

[0062] Composition Example 4 One-component silicone rubber composition 4 was prepared in the same manner as in Composition Example 1, except that 0.05 parts by mass of "catalyst 4" was used in place of "catalyst 1."

[0063] Comparative Composition Example 1 One-component silicone rubber composition 5 was produced in the same manner as in Composition Example 1, except that 0.05 parts by mass of "Catalyst 5" was used instead of "Catalyst 1".

[0064] Comparative Composition Example 2 One-component silicone rubber composition 6 was produced in the same manner as in Composition Example 1, except that 0.05 parts by mass of "Catalyst 6" was used in place of "Catalyst 1."

[0065] Comparative Composition Example 3 One-component silicone rubber composition 7 was produced in the same manner as in Composition Example 1, except that 0.05 parts by mass of "Catalyst 7" was used in place of "Catalyst 1".

[0066] Comparative Composition Example 4 One-component silicone rubber composition 8 was produced in the same manner as in Composition Example 1, except that 0.05 parts by mass of "catalyst 8" was used instead of "catalyst 1."

[0067] [Comparative Composition Example 5] One-component silicone rubber composition 9 was produced in the same manner as in Composition Example 1, except that 0.05 parts by mass of a platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex having 1% Pt atoms was used instead of "Catalyst 1."

[0068] [Tests] Table 2 shows the results obtained in the above Composition Examples 1 to 4 and Comparative Composition Examples 1 to 5.

[0069]

[0070] [Composition Evaluation] The platinum-phosphite complex-containing hydrosilylation catalysts obtained in Examples 1 to 4 satisfy the requirements of the present invention, and the curable organopolysiloxane compositions using these catalysts in Examples 1 to 4 also exhibit good storage stability at 23°C. In contrast, the platinum-phosphite complex-containing hydrosilylation catalysts in Comparative Examples 1 to 4 failed the catalyst evaluation due to crystallization at 23°C. Furthermore, because the required amount of catalyst had to be blended while removing the crystalline components during catalyst addition, they also failed in terms of workability. However, the curable organopolysiloxane compositions using these catalysts exhibited good storage stability. Therefore, if the catalyst were liquid at 23°C, workability during catalyst addition would also be improved. Furthermore, the platinum-phosphite complex-containing hydrosilylation catalyst of Comparative Example 4 was obtained without the use of a hydrocarbon solvent. As a result, complex formation between the phosphite ester compound and platinum was poor, resulting in reduced storage stability for the curable silicone composition prepared using it. Comparative Example 5 is an example of a curable organopolysiloxane composition in which an organic solvent-free platinum compound selected from the group consisting of complexes of chloroplatinic acid or chloroplatinic acid salts and vinyl group-containing siloxanes was directly used, without forming a complex between platinum and the phosphite ester or associating with the siloxane compound. The curable organopolysiloxane composition prepared using this catalyst resulted in reduced storage stability. The above results demonstrate that the curable organopolysiloxane composition prepared using the platinum-phosphite complex-containing hydrosilylation catalyst obtained according to the present invention exhibits excellent performance in terms of improved workability and storage stability.

[0071] This specification includes the following aspects: [1]: (A) Platinum and the following general formula (1) (In the formula, R 1(B) a silane compound represented by the following general formula (2) and / or a partial hydrolyzate thereof; (In the formula, R 2 represents an alkenyl group having 2 to 10 carbon atoms, and R 3 is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms. X is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms or OR 3 The hydrosilylation catalyst is an association of the component (A) and the component (B), does not contain an organic solvent, and is liquid at 23°C. [2]: The component (B) is a platinum-phosphite complex-containing hydrosilylation catalyst characterized in that it is an association of the component (A) and the component (B), does not contain an organic solvent, and is liquid at 23°C. 2

[0023] The platinum-phosphite complex-containing hydrosilylation catalyst according to [1], wherein the alkoxysilane derivative is a platinum-phosphite complex-containing hydrosilylation catalyst, wherein R is a vinyl group. [3]: A curable organopolysiloxane composition comprising the platinum-phosphite complex-containing hydrosilylation catalyst according to [1] or [2]. [4]: ​​The curable organopolysiloxane composition according to [3], wherein the curable organopolysiloxane composition does not contain an organic solvent. [5]: An article comprising a cured product of the curable organopolysiloxane composition according to [3] or [4]. [6]: A method for producing a platinum-phosphite complex-containing hydrosilylation catalyst, comprising the following steps (a) to (d): (a) preparing a solution in which a phosphite compound represented by the following general formula (1) is dissolved in a hydrocarbon solvent having a boiling point of 80°C or less; (In the formula, R 1is a hydrogen atom or a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms.) (b) adding an organic solvent-free platinum compound selected from the group consisting of platinum chloride, chloroplatinic acid, or a complex of a chloroplatinate with a vinyl group-containing siloxane to the solution and dispersing the compound to prepare a solution containing a platinum-phosphite complex; (c) adding a silane compound represented by the following general formula (2) and / or a partial hydrolyzate thereof to the solution obtained in steps (a) and (b) above and dispersing the compound to prepare a solution containing an association product of at least a portion of the platinum-phosphite complex and the silane compound represented by the following general formula (2) and / or a partial hydrolyzate thereof; (In the formula, R 2 represents an alkenyl group having 2 to 10 carbon atoms, and R 3 is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms. X is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms or OR 3 (d) a step of removing the hydrocarbon solvent from the solution obtained in the step (c). [7]: The method for producing a platinum-phosphite complex-containing hydrosilylation catalyst according to [6], characterized in that in the step (c), the silane compound and / or the partial hydrolyzate thereof is added so that the number of moles of alkenyl groups in the silane compound and / or the partial hydrolyzate thereof is within the range of 0.01 to 500 times that of one platinum atom in the platinum compound.

[0072] The present invention is not limited to the above-described embodiments. The above-described embodiments are merely examples, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and that exhibits similar effects is included within the technical scope of the present invention.

[0073] The platinum-phosphite complex-containing hydrosilylation catalyst of the present invention, even though conventional platinum-phosphite complex-containing hydrosilylation catalysts tend to form crystals, can maintain liquid properties at 23°C without the use of organic solvents. This improves the stability of the hydrosilylation catalyst itself, improves workability when producing curable organopolysiloxane compositions using this catalyst, and enables the production of highly safe curable organopolysiloxane compositions that are free of hydrocarbon organic solvents. This platinum-phosphite complex-containing hydrosilylation catalyst therefore has very little adverse effect on the human body. Furthermore, the resulting hydrocarbon-free curable organopolysiloxane compositions exhibit stable properties and characteristics even when exposed to temperatures above room temperature for extended periods of time, making them suitable for a wide range of applications, including electrical equipment, automobiles, construction, medicine, and food.

Claims

1. (A) Platinum and the following general formula (1) (In the formula, R 1 is a hydrogen atom or a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms; and (B) a silane compound represented by the following general formula (2) and / or a partial hydrolyzate thereof, (In the formula, R 2 represents an alkenyl group having 2 to 10 carbon atoms; R 3 is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms. X is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms or OR 3 The hydrosilylation catalyst is an association of the component (A) and the component (B), does not contain an organic solvent, and is liquid at 23° C.

2. The component (B) is 2 2. The platinum-phosphite complex-containing hydrosilylation catalyst according to claim 1, which is an alkoxysilane derivative in which R is a vinyl group.

3. A curable organopolysiloxane composition comprising the platinum-phosphite complex-containing hydrosilylation catalyst according to claim 1 or 2.

4. The curable organopolysiloxane composition according to claim 3, which contains no organic solvent.

5. An article comprising the cured product of the curable organopolysiloxane composition according to claim 3.

6. A method for producing a platinum-phosphite complex-containing hydrosilylation catalyst, comprising the following steps (a) to (d): (a) preparing a solution in which a phosphite compound represented by the following general formula (1) is dissolved in a hydrocarbon solvent having a boiling point of 80° C. or lower; (In the formula, R 1is a hydrogen atom or a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms; (b) adding to the solution a platinum compound not containing an organic solvent, selected from the group consisting of platinum chloride, chloroplatinic acid or a complex of a chloroplatinate with a vinyl group-containing siloxane, and dispersing the compound to prepare a solution containing a platinum-phosphite complex; (c) adding to the solution obtained in steps (a) to (b) a silane compound represented by the following general formula (2) and / or a partial hydrolysate thereof, and dispersing the compound to prepare a solution containing an association product of at least a portion of the platinum-phosphite complex and a silane compound represented by the following general formula (2) and / or a partial hydrolysate thereof; (In the formula, R 2 represents an alkenyl group having 2 to 10 carbon atoms; R 3 is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms. X is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms or OR 3 (d) removing the hydrocarbon solvent from the solution obtained in the step (c).

7. The method for producing a platinum-phosphite complex-containing hydrosilylation catalyst according to claim 6, characterized in that in step (c), the silane compound and / or partial hydrolysate thereof is added so that the number of moles of alkenyl groups in the silane compound and / or partial hydrolysate thereof falls within the range of 0.01 to 500 times the number of moles of one platinum atom in the platinum compound.

Citation Information

Patent Citations

  • Curable silicone gel composition and silicone gel cured product

    JP2021042323A

  • One-pack type curable silicone gel composition and cured silicone gel

    WO2021014970A1

  • High-temperature-resistance, anti-aging and high-transparent organic silica gel

    CN108587454A

  • Organosilicon composition for ultraviolet LED packaging and preparation method thereof

    CN109749701A

  • Platinum-phosphite ester complex-containing hydrosilylation catalyst, method for preparing same, method for inhibiting crystallization of platinum-phosphite ester complex-containing hydrosilylation catalyst, and curable organopolysiloxane composition and article

    WO2023013443A1

Cited By

  • Hydrosilylation reaction catalyst and preparation method thereof

    CN121732244A