Anode active material for lithium secondary battery, manufacturing method therefor, and lithium secondary battery containing comprising same
Patent Information
- Application Number
- PCT/KR2024/005031
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-19
- Filing Date
- 2024-04-15
- Publication Date
- 2024-10-24
Smart Images

Figure KR2024005031_24102024_PF_FP_ABST
Abstract
Description
Negative active material for lithium secondary battery, method for producing same, and lithium secondary battery including same
[0001] The present invention relates to an anode active material for a lithium secondary battery, a method for producing the same, and a lithium secondary battery comprising the same, and more specifically, to an anode active material for a lithium secondary battery comprising a carbon-based active material and a silicon-based active material, a method for producing the same, and a lithium secondary battery comprising the same.
[0002]
[0003] As technological developments and demand for mobile devices increase, the demand for rechargeable, miniaturized, and high-capacity secondary batteries is rapidly increasing. Recently, the use of secondary batteries as power sources for hybrid electric vehicles (HEVs) and electric vehicles (EVs) is becoming a reality.
[0004] Accordingly, much research is being conducted on secondary batteries that can meet various needs, and in particular, the demand for lithium secondary batteries with high energy density, high discharge voltage, and output is increasing. Furthermore, lithium secondary batteries used in electric vehicles must have the characteristics of high energy density and the ability to generate high output in a short period of time. In addition, they must be able to be used for more than 10 years under harsh conditions where high-current charging and discharging are repeated in a short period of time. Therefore, they inevitably require output characteristics and long-life characteristics that are far superior to those of existing small lithium secondary batteries.
[0005] In particular, with the recent increase in demand for high-density energy batteries, active research is being conducted on methods to increase capacity by using silicon-based materials such as Si / C or SiOx, which have a capacity more than 10 times greater than graphite-based materials, together with the anode active material. However, in the case of silicon-based materials, which are high-capacity materials, although the capacity characteristics are superior to the conventional graphite, there is a problem that the volume rapidly expands during the charging process, which cuts off the conductive path, deteriorates the battery characteristics, and consequently, the life characteristics of the battery deteriorate.
[0006] Accordingly, research is needed on graphite and silicon-based negative electrode active materials that can appropriately secure both battery capacity and lifespan characteristics.
[0007]
[0008] Accordingly, one object of the present invention is to provide a carbon-based and silicon-based mixed negative electrode active material capable of improving both capacity and life characteristics of a battery, a method for producing the same, and a lithium secondary battery including the same.
[0009]
[0010] One embodiment of the present invention comprises a mixture of a carbon-based active material and a silicon-based active material, and has a pressure of 700 to 1300 kgf / cm 2 Shrinkage density at compression pressures in the range of 0.80 g / cm 3 The present invention provides a negative active material for a lithium secondary battery, wherein the shrinkage density is defined as the difference between the pellet density and the tap density.
[0011] The above negative active material for lithium secondary batteries is 1000 kgf / cm 2 At a compression pressure of 0.90 g / cm, the shrinkage density is 3 It could be strange.
[0012] The above negative active material for lithium secondary batteries has a density of 1300 kgf / cm 2 Shrinkage density at a compression pressure of 1.00 g / cm 3 It could be strange.
[0013] The above carbon-based active material may be natural graphite.
[0014] The sphericity of the above carbon-based active material may be 0.87 or more.
[0015] The above carbon-based active material may be oxidized.
[0016] The above silicon-based active material may be silicon.
[0017] The above silicon-based active material may have a circularity of 0.931 or more.
[0018] The above silicon-based active material may have a crystal grain size of 175 nm or less.
[0019] The above silicon-based active material has a strain of 10×10 -5 It could be strange.
[0020] The content of the above silicon-based active material may be 4 to 6 wt% based on the total weight of the mixture.
[0021]
[0022] Another embodiment of the present invention is a method for manufacturing an anode active material, comprising the steps of: preparing a carbon-based active material; preparing a silicon-based active material by first crushing, second crushing, and third crushing of a silicon-based active material raw material; and mixing the carbon-based active material and the silicon-based active material to form a mixture, wherein the anode active material has a density of 700 to 1300 kgf / cm. 2 Shrinkage density at compression pressures in the range of 0.80 g / cm 3 The present invention provides a method for manufacturing a negative electrode active material for a lithium secondary battery, wherein the above shrinkage density is defined as the difference between the pellet density and the tap density.
[0023] In the step of preparing the above carbon-based active material, the carbon-based active material may be natural graphite.
[0024] In the step of preparing the above carbon-based active material, the carbon-based active material may have a sphericity of 0.87 or more.
[0025] After the step of preparing the above carbon-based active material, a step of performing oxidation treatment by heat treatment on the prepared carbon-based active material under an air atmosphere may be further included.
[0026] The above heat treatment can be performed at a temperature of 500 to 700°C.
[0027] The above heat treatment can be performed for 30 minutes to 6 hours.
[0028] In the step of forming the mixture, the content of the silicon-based active material may be 4 to 6 wt% based on the total weight of the mixture.
[0029]
[0030] Another embodiment of the present invention provides a lithium secondary battery comprising a positive electrode; a negative electrode; an electrolyte; and a separator, wherein the negative electrode comprises the negative electrode active material described above.
[0031]
[0032] According to one embodiment of the present invention, a negative active material for a lithium secondary battery can not only improve the capacity of the battery by further including a silicon-based active material in addition to a carbon-based active material, but also minimize deterioration of the life characteristics of the battery as the shrinkage density is sufficiently large.
[0033]
[0034] Figure 1 is a schematic diagram of a negative electrode active material for a lithium secondary battery according to one embodiment of the present invention.
[0035] Figure 2 is a graph showing the shrinkage density measurement results of negative electrode active materials manufactured according to Examples 1 to 3 and Comparative Examples 1 to 4.
[0036] Figure 3 is a graph showing the results of evaluating the life characteristics of lithium secondary batteries manufactured according to Examples 1 to 3 and Comparative Examples 1 to 4.
[0037]
[0038] The terms first, second, and third, etc., are used to describe, but are not limited to, various parts, components, regions, layers, and / or sections. These terms are used only to distinguish one part, component, region, layer, or section from another part, component, region, layer, or section. Accordingly, a first part, component, region, layer, or section described below may be referred to as a second part, component, region, layer, or section without departing from the scope of the present invention.
[0039] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the present invention. As used herein, the singular forms "singular" and "comprising" include plural forms as well, unless the context clearly dictates otherwise. The word "comprising" as used herein specifies a particular feature, region, integer, step, operation, element, and / or component, but does not exclude the presence or addition of other features, regions, integers, steps, operations, elements, and / or components.
[0040] When a part is referred to as being "on" or "over" another part, it can be directly on or over the other part, or there may be other parts intervening. Conversely, when a part is referred to as being "directly on" another part, there are no other parts intervening.
[0041] Although not defined otherwise, all terms, including technical and scientific terms, used herein have the same meaning as commonly understood by those of ordinary skill in the technical field to which the present invention pertains. Terms defined in commonly used dictionaries are further interpreted to have meanings consistent with the relevant technical literature and the present disclosure, and are not to be construed as ideal or overly formal unless otherwise defined.
[0042] Also, unless otherwise stated, % means weight%, and 1 ppm is 0.0001 weight%.
[0043] In this specification, the term "combination(s) thereof" described in the expression in the Makushi format means one or more mixtures or combinations selected from the group consisting of the components described in the expression in the Makushi format, and means including any one or more selected from the group consisting of said components.
[0044] Hereinafter, embodiments of the present invention will be described in detail so that those skilled in the art can easily implement them. However, the present invention may be implemented in various different forms and is not limited to the embodiments described herein.
[0045]
[0046] 1. Negative active material
[0047] FIG. 1 is a schematic diagram of an anode active material for a lithium secondary battery according to one embodiment of the present invention. Hereinafter, an anode active material for a lithium secondary battery according to one embodiment of the present invention will be described with reference to FIG. 1.
[0048] One embodiment of the present invention comprises a mixture of a carbon-based active material and a silicon-based active material, and has a pressure of 700 to 1300 kgf / cm 2 Shrinkage density at compression pressures in the range of 0.80 g / cm 3 The present invention provides a negative active material for a lithium secondary battery, wherein the shrinkage density is defined as the difference between the pellet density and the tap density.
[0049] According to one embodiment of the present invention, a negative active material for a lithium secondary battery comprises a mixture of a carbon-based active material and a silicon-based active material. By further including a silicon-based active material, which has a capacity at least 10 times greater than the carbon-based active material, the capacity characteristics of the battery can be improved. However, if the silicon-based active material is further included, the electrode volume rapidly expands during charging, cutting off the conductive path, thereby deteriorating battery characteristics and significantly deteriorating the lifespan characteristics as charge and discharge progress.
[0050] The inventors of the present invention have conducted repeated research on a method for minimizing the deterioration of life characteristics that occurs when the silicon-based active material is further included, and as a result, have discovered that when the shrinkage density of the active material is sufficiently large, the volume expansion rate of the electrode is reduced, thereby improving the life characteristics of the battery, thereby completing the present invention.
[0051]
[0052] According to one embodiment of the present invention, the negative active material for a lithium secondary battery has a density of 700 to 1300 kgf / cm 2 Shrinkage density at compression pressures in the range of 0.80 g / cm 3 and more specifically 0.805 g / cm 3 or more than 0.81 g / cm 3 It could be strange.
[0053] In this specification, “shrinkage density” is defined as the difference between the pellet density and the tap density. Here, “pellet density” is defined as the difference between the pellet density and the tap density for a diameter of 2 cm. 2It is defined as the density measured after applying a specific compression pressure to 2g of active material powder in a circular mold. As can be seen from the definition above, this pellet density can vary depending on the value of the compression pressure applied to the active material powder, and generally increases as the compression pressure increases. “Tapped density” is defined as the density measured after tapping 3000 cycles @ 284 cycles / min after placing 10g of active material powder in a 50mL container based on ASTM-B527. Unlike the pellet density, the tapped density has a constant value. The pellet density has a larger value than the tapped density.
[0054] According to one embodiment of the present invention, since the negative electrode active material for a lithium secondary battery has a sufficiently large shrinkage density as described above, the pressure generated by the volume expansion of the silicon negative electrode material during charge / discharge of the negative electrode is absorbed by the carbon-based active material as it shrinks, thereby reducing the volume expansion rate of the electrode during charge / discharge. As a result, the life characteristics of the battery can be improved.
[0055] More specifically, the negative active material for the lithium secondary battery has a density of 700 kgf / cm 2 Shrinkage density at a compression pressure of 0.80 g / cm 3 , 0.805 g / cm 3 or 0.81 g / cm 3 It could be strange.
[0056] - More specifically, the negative active material for the lithium secondary battery has a density of 800 kgf / cm 2 The shrinkage density at a compression pressure of 0.82 g / cm 3 , 0.835 g / cm 3 or 0.85 g / cm 3 It could be strange.
[0057] More specifically, the negative active material for the lithium secondary battery has a density of 900 kgf / cm 2 At a compression pressure of 0.86 g / cm, the shrinkage density is 3, 0.875 g / cm 3 or 0.89 g / cm 3 It could be strange.
[0058] More specifically, the negative active material for the lithium secondary battery has a density of 1000 kgf / cm 2 At a compression pressure of 0.90 g / cm, the shrinkage density is 3 , 0.915 g / cm 3 or 0.92 g / cm 3 It could be strange.
[0059] More specifically, the negative active material for the lithium secondary battery has a density of 1200 kgf / cm 2 At a compression pressure of 0.96 g / cm, the shrinkage density is 3 , 0.975 g / cm 3 or 0.98 g / cm 3 It could be strange.
[0060] More specifically, the negative active material for the lithium secondary battery has a density of 1300 kgf / cm 2 Shrinkage density at a compression pressure of 1.00 g / cm 3 or 1.01 g / cm 3 It could be strange.
[0061] More specifically, the negative active material for the lithium secondary battery has a tap density of 0.80 to 0.95 g / cm 3 It could be.
[0062]
[0063] The above carbon-based active material may be natural graphite. When the carbon-based active material is natural graphite, the shrinkage density of the active material can be more easily achieved within the aforementioned numerical range, and the resulting battery performance improvement effect can be more effectively achieved.
[0064] The above carbon-based active material may have a sphericity of 0.87 or higher. When the sphericity of the carbon-based active material satisfies the above range, the adhesion between the active material and the current collector is improved, which has advantages in the manufacturing process, and the capacity and output characteristics of the battery can be further improved. In the present specification, “sphericity” is a numerical expression of the degree to which a particle is close to a sphere, and refers to a value obtained by dividing the perimeter of a circle having the same area as a particle projection shape by the actual perimeter of the particle projection shape using a flow-type particle analysis device. This sphericity can be measured using an analyzer for obtaining an optical image (Fluid Imaging Technologies, Flowcam 8100) and analysis S / W (visual spreadsheet).
[0065]
[0066] In particular, the carbon-based active material may be oxidized. Conventionally, in order to improve the lifespan characteristics of carbon-based active materials, low-crystalline carbon materials such as soft carbon or hard carbon were generally coated on the carbon-based active material. However, the carbon-based active material according to the present invention may be oxidized rather than coated with a low-crystalline carbon material. As the carbon-based active material undergoes oxidation treatment, internal pores increase, weakening the hardness of the graphite. Ultimately, a difference in density due to tapping of the powder and a density due to compression occurs, and this difference means that the expansion pressure generated during charge and discharge of the mixed silicon can be absorbed. Therefore, the shrinkage density of the active material can be more easily achieved within the aforementioned numerical range, and the battery performance improvement effect can be more preferably achieved. On the other hand, when the carbon-based active material is coated with a low-crystalline carbon material, the shrinkage density of the active material cannot be easily achieved within the aforementioned numerical range, which is unsuitable.
[0067]
[0068] The above silicon-based active material may be silicon particles. When a silicon-based active material is selected as the material, the shrinkage density of the active material can be more easily achieved within the aforementioned numerical range, and thus the battery performance improvement effect can be more preferably achieved.
[0069]
[0070] Meanwhile, the above silicon-based active material may have a circularity of 0.931 or more.
[0071] In this specification, "circularity" is a numerical expression of the degree to which a particle is close to being circular. It refers to the value obtained by dividing the perimeter of the particle shape by the perimeter of a circle with an equivalent area in an individual 2D image for each particle using an image analysis device. The data is collected, analyzed, and displayed. This circularity can be measured using an analyzer for optical image acquisition (Malvernpanalytical, Morphologi 4).
[0072]
[0073] In addition, the silicon-based active material may have a crystal grain size of 175 nm or less, more specifically, 170 nm or less.
[0074] In this specification, the “crystal grain size” can be measured by analyzing X-ray diffraction data of a cross-section of an active material using the Rietveld refinement method. For example, the crystal grain size can be obtained by performing X-ray diffraction analysis using Bruker’s D8 Discover with GADDS XRD equipment under the following conditions to obtain XRD data, and then processing the XRD data using Bruker’s DIFFRAC.TOPAS program. At this time, the half width is set to be measured using the Caglioti equation.
[0075] <X-선 회절 분석 조건>
[0076] Light source: Cu target, 45 kV, 40 mA output, wavelength = 1.54 Å
[0077] Detector: GaliPIX3D
[0078] Sample preparation: Approximately 2 g of sample was placed in a 2 cm diameter holder and loaded onto the rotation stage.
[0079] Measurement time: approximately 20 minutes
[0080] Measurement range: 2θ=10°~90°
[0081]
[0082] In addition, the above silicon-based active material has a strain of 10×10 -5 It could be more than 10.3 × 10, more specifically -5- It could be.
[0083] In this specification, “strain” is a value measured through Rietveld refinement analysis of X-ray diffraction data, and is a lattice spacing It represents the average deviation and is a value that indicates the degree of deformation of the crystal lattice and satisfies the following equation.
[0084]
[0085] At this time, represents the full width at half maximum of the profile component associated with the microstrain expansion.
[0086]
[0087] When the circularity, crystal grain size, and strain of the silicon-based active material satisfy the above ranges, the rigidity and volume expansion characteristics of the powder against compression pressure are determined, so that the shrinkage density of the active material can be more easily implemented within the aforementioned numerical range, and the battery performance improvement effect can be more preferably implemented accordingly.
[0088] These various properties of silicon-based active materials can be readily obtained by performing a multi-stage grinding process of first, second, and third grinding of the silicon-based active material raw material during the manufacturing process. This will be described in more detail in the manufacturing method of the negative electrode active material described below.
[0089]
[0090] The content of the above silicon-based active material may be 3 to 7 wt% based on the total weight of the mixture, and more specifically, 4 to 6 wt%. When the content of the silicon-based active material satisfies the above range, the simultaneous implementation effects of the capacity and life characteristics of the battery can be more preferably implemented. More specifically, if the content of the silicon-based active material is too low, the effect of improving the battery capacity characteristics may be minimal, and if the content of the silicon-based active material is too high, the electrode expansion rate due to charge and discharge may become too large, and the effect of improving the battery life characteristics may be minimal.
[0091]
[0092] The above-mentioned negative active material may have an average particle diameter (D50) of 10 to 30 μm. In this specification, the average particle diameter (D50) may be defined as a particle diameter corresponding to 50% of the volume accumulation amount in a particle diameter distribution curve. The average particle diameter (D50) may be measured using, for example, a laser diffraction method.
[0093] The above negative active material has a specific surface area of 3 to 6 m 2 / g may be. In this specification, the specific surface area of the active material can be measured using the BET method (Surface area and Porosity analyzer) (Micromeritics, ASAP2020) for the active material powder.
[0094] When the average particle size and specific surface area of the negative active material satisfy the above range, battery performance can be more preferably implemented.
[0095]
[0096] 2. Method for manufacturing negative active material
[0097] Another embodiment of the present invention is a method for producing an anode active material, comprising the steps of: preparing a carbon-based active material; preparing a silicon-based active material by first crushing, second crushing, and third crushing of a silicon-based active material raw material; and mixing the carbon-based active material and the silicon-based active material to form a mixture, wherein the anode active material has a density of 700 to 1300 kgf / cm. 2 Shrinkage density at compression pressures in the range of 0.80 g / cm 3 The present invention provides a method for manufacturing a negative electrode active material for a lithium secondary battery, wherein the above shrinkage density is defined as the difference between the pellet density and the tap density.
[0098] A method for manufacturing a negative active material according to another embodiment of the present invention will be described in more detail step by step.
[0099]
[0100] First, prepare a carbon-based active material.
[0101] The above carbon-based active material may be natural graphite.
[0102] At this time, the carbon-based active material may be obtained through a spheroidization process.
[0103] The above spheroidization may be performed by a general method in the art for spheroidizing plate-shaped or flake-shaped carbon-based active material raw material powder.
[0104]
[0105] In particular, after the step of preparing the carbon-based active material, a step of performing oxidation treatment by heat treatment on the prepared carbon-based active material under an air atmosphere may be further included. The technical significance of performing oxidation treatment on the carbon-based active material is as described above, and thus is omitted.
[0106] At this time, the heat treatment can be performed at a temperature of 500 to 700°C, and more specifically, can be performed at a temperature of 550 to 650°C. When the heat treatment temperature satisfies the above range, the effect according to the oxidation treatment described above can be more preferably implemented. More specifically, if the heat treatment temperature is too low, the oxidation reactivity by oxygen may be lowered, which may lower the shrinkage density of the active material, and if the heat treatment temperature is too high, there may be problems of deterioration of battery characteristics due to structural collapse of the spherical graphite due to the violent oxidation reaction and increased costs due to low yield.
[0107] In addition, the heat treatment can be performed for 30 minutes to 6 hours, and more specifically, can be performed for 1 hour to 5 hours. When the heat treatment time satisfies the above range, the effect according to the oxidation treatment described above can be more preferably implemented. More specifically, if the heat treatment time is too short, the natural graphite is less oxidized, the increase in internal pores is reduced, and eventually the effect of absorbing the expansion of silicon is reduced, which may cause the lifespan of the battery to deteriorate, and if the heat treatment time is too long, the high BET of the active material may cause high viscosity during the electrode manufacturing process, which may lower the processability and reduce the yield, thereby increasing the manufacturing cost, or the side reaction with the electrolyte may be severe, which may cause a problem of deterioration in the battery life characteristics.
[0108]
[0109]
[0110] Next, the silicon-based active material raw material is sequentially subjected to first, second, and third grinding to prepare a silicon-based active material. By performing the first, second, and third grinding, the circularity, grain size, and strain of the silicon-based active material are controlled within appropriate ranges, so that the shrinkage density of the original active material can be more preferably implemented.
[0111] More specifically, the silicon-based active material raw material may be metallic silicon powder, and in this case, the metallic silicon powder may contain 98% or more of silicon and other impurities based on the total weight.
[0112] The above first crushing can be performed using crushing equipment commonly used in the art, and is not particularly limited. For example, the above first crushing can be performed using a jaw crusher, but is not limited thereto.
[0113] The second pulverization can be performed using pulverization equipment commonly used in the art, and is not particularly limited. For example, the second pulverization can be performed using one or more selected from a jet mill, a ball mill, a stirred media mill, a roll mill, a hammer mill, a pin mill, a disk mill, a colloid mill, and an atomizer mill, but is not limited thereto.
[0114] At this time, the second crushing may be performed two or more times. By performing the second crushing multiple times in this way, the circularity and strain of the silicon-based active material can be further improved, and the crystal grain size can be reduced, so that the battery performance improvement effect can be maximized.
[0115] The third pulverization can be performed using pulverization equipment commonly used in the art, and is not particularly limited. For example, the third pulverization can be performed using one or more selected from a jet mill, a spiral jet mill, a ball mill, a stirred media mill, a roll mill, a hammer mill, a pin mill, a disk mill, a colloid mill, and an atomizer mill, but is not limited thereto.
[0116]
[0117]
[0118] Next, the carbon-based active material and the silicon-based active material are mixed to form a mixture. The negative active material according to the present invention, which is the mixture thus formed, has a strength of 700 to 1300 kgf / cm. 2 Shrinkage density at compression pressures in the range of 0.80 g / cm 3 That is all. The technical significance of the shrinkage density of the negative active material according to the present invention satisfying the above range and the more detailed shrinkage density range are as described above, so they are omitted.
[0119] At this time, the content of the silicon-based active material may be 3 to 7 wt% based on the total weight of the mixture, and more specifically, 4 to 6 wt%.
[0120]
[0121] 3. Lithium secondary battery
[0122] Another embodiment of the present invention provides a lithium secondary battery comprising a positive electrode; a negative electrode; a separator; and an electrolyte, wherein the negative electrode comprises the negative electrode active material described above.
[0123] In addition, the lithium secondary battery may optionally further include a battery container that houses an electrode assembly of a positive electrode, a negative electrode, and a separator, and a sealing member that seals the battery container.
[0124]
[0125] The above negative electrode may more specifically include a negative electrode current collector; and a negative electrode active material layer positioned on the negative electrode current collector and including the above-described negative electrode active material for a lithium secondary battery.
[0126] The negative electrode current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. can be used. In addition, the negative electrode current collector can typically have a thickness of 3 to 500 ㎛, and like the positive electrode current collector, fine unevenness can be formed on the surface of the current collector to strengthen the bonding strength of the negative electrode active material. For example, it can be used in various forms such as a film, a sheet, a foil, a net, a porous body, a foam, a non-woven fabric, etc.
[0127] The above negative electrode active material layer may optionally include a binder and / or a conductive material together with the negative electrode active material.
[0128] The above binder serves to improve the adhesion between negative electrode active material particles and the adhesive strength between the negative electrode active material and the negative electrode current collector. Specific examples thereof include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one of these may be used alone or a mixture of two or more thereof. The binder may be included in an amount of 1 to 30 wt% based on the total weight of the negative electrode active material layer.
[0129] The conductive material is used to provide conductivity to the electrode, and in the battery to be formed, as long as it does not cause a chemical change and has electronic conductivity, it can be used without any special restrictions. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, and carbon fiber; metal powder or metal fiber such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and the like. One type alone or a mixture of two or more types of these may be used. The conductive material may typically be included in an amount of 1 to 30 wt% based on the total weight of the negative electrode active material layer.
[0130] A negative electrode for a lithium secondary battery according to one embodiment of the present invention can be manufactured according to a conventional negative electrode manufacturing method, except that the negative electrode active material described above is used.
[0131] Specifically, the composition for forming a negative electrode active material layer, including the aforementioned negative electrode active material and optionally a binder, a conductive agent, and a solvent, can be applied onto a negative electrode current collector, followed by rolling and drying. At this time, the types and contents of the negative electrode active material, binder, and conductive agent are as described above.
[0132] The solvent may be a solvent generally used in the relevant technical field, such as dimethylsulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or water. One of these may be used alone or a mixture of two or more thereof may be used. The amount of the solvent used is sufficient to dissolve or disperse the negative electrode active material, conductive material, and binder, taking into account the coating thickness and manufacturing yield of the slurry, and to have a viscosity that can exhibit excellent thickness uniformity when applied thereafter for manufacturing the negative electrode.
[0133] Alternatively, the negative electrode may be manufactured by casting the composition for forming the negative electrode active material layer on a separate support, then peeling the film from the support and laminating the resulting film on a negative electrode current collector.
[0134]
[0135] The above positive electrode may include a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector, and the positive electrode active material layer may include a positive electrode active material.
[0136] The above positive electrode active material can be used without any special restrictions as long as it is commonly used in the art.
[0137]
[0138] The above separator separates the positive and negative electrodes and provides a passage for lithium ions to move. Any separator commonly used as a separator in lithium secondary batteries can be used without any particular restrictions. In particular, a separator having low resistance to ion movement of the electrolyte and excellent electrolyte moisture absorption capacity is preferable. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof, may be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high-melting-point glass fiber, polyethylene terephthalate fiber, etc. may be used. In addition, a coated separator containing a ceramic component or a polymer material to secure heat resistance or mechanical strength may be used, and may optionally be used in a single-layer or multi-layer structure.
[0139]
[0140] The above electrolyte may include, but is not limited to, organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the manufacture of lithium secondary batteries.
[0141] Specifically, the organic liquid electrolyte may include an organic solvent and a lithium salt.
[0142] The organic solvent may be used without any particular limitation as long as it can serve as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the organic solvent may include ester solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether solvents such as dibutyl ether or tetrahydrofuran; ketone solvents such as cyclohexanone; aromatic hydrocarbon solvents such as benzene and fluorobenzene; Carbonate solvents such as dimethylcarbonate (DMC), diethylcarbonate (DEC), methylethylcarbonate (MEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); alcohol solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (wherein R is a C2 to C20 linear, branched, or cyclic hydrocarbon group, and may include a double-bonded aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes can be used. Among these, a carbonate solvent is preferable, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate, etc.) having high ionic conductivity and high dielectric constant that can improve the charge / discharge performance of the battery and a linear carbonate compound having low viscosity (e.g., ethyl methyl carbonate, dimethyl carbonate, or diethyl carbonate, etc.) is more preferable.In this case, the performance of the electrolyte may be improved when the cyclic carbonate and the chain carbonate are mixed and used in a volume ratio of about 1:1 to about 1:9.
[0143] The lithium salt may be used without any particular limitation as long as it is a compound capable of providing lithium ions used in a lithium secondary battery. Specifically, the lithium salt may be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAl04, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2. LiCl, LiI, or LiB(C2O4)2. It is preferable that the concentration of the lithium salt be used within the range of 0.1 to 2.0 M. When the concentration of the lithium salt is within the above range, the electrolyte can exhibit excellent electrolyte performance because it has appropriate conductivity and viscosity, and lithium ions can move effectively.
[0144] In addition to the electrolyte components, the electrolyte may further include one or more additives, such as haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethylphosphite, triethanolamine, cyclic ethers, ethylene diamine, n-glyme, hexamethylphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride, for the purpose of improving the life characteristics of the battery, suppressing battery capacity decrease, and improving the discharge capacity of the battery. At this time, the additives may be included in an amount of 0.1 to 5 wt% based on the total weight of the electrolyte.
[0145]
[0146] Hereinafter, embodiments of the present invention will be described in more detail through examples. However, the following examples are merely preferred embodiments of the present invention, and the present invention is not limited to the following examples.
[0147]
[0148] Example 1
[0149] (1) Manufacturing of negative electrode active material
[0150] (Preparation of carbon-based active material) Spherical natural graphite particles with an average particle diameter (D50) of 17 μm were heat-treated in an air atmosphere at 600°C for 3 hours in a continuous rotary kiln, and then subjected to oxidation treatment, followed by classification through a 45 μm sieve.
[0151] (Preparation of Silicon-Based Active Material) Metallurgical silicon powder was first crushed using conventional crushing equipment. Subsequently, a first crushing and a second crushing were performed using a different type of conventional crushing equipment. A third crushing was then performed using a different type of conventional crushing equipment. Subsequently, silicon particles were prepared by ultrasonic classification.
[0152] (Mixing) The carbon-based active material and silicon-based active material prepared above were mixed to form a mixture, and the content of the silicon-based active material was set to 5 wt% based on the total weight of the mixture to manufacture a negative electrode active material.
[0153] (2) Cathode manufacturing
[0154] The above-mentioned manufactured negative active material, styrene butadiene rubber (SBR) as a binder, and carboxymethyl cellulose (CMC) as a thickener were prepared, and these were mixed at a mass ratio of 98.0:1.0:1.0 (negative active material:binder:thickener), and then dispersed in distilled water from which ions had been removed to prepare a negative active material composition. The composition was applied to a Cu-foil current collector, and then dried and rolled. During rolling, the pressure conditions were varied to maintain an electrode density of 1.60±0.05 g / cm. 3 The cathode was prepared.
[0155] (3) Lithium secondary battery manufacturing
[0156] A coin-type 2032 half-cell was manufactured using the above-mentioned cathode as a working electrode and metallic lithium as a counter electrode. At this time, a separator made of a porous polypropylene film was inserted between the working electrode and the counter electrode, and the electrolyte used was a 7:3 volume ratio mixed solution of diethyl carbonate (DEC) and ethylene carbonate (EC) in which 1 M concentration of LiPF6 was dissolved.
[0157]
[0158] Example 2
[0159] In the carbon-based active material preparation step, a negative electrode active material and a lithium secondary battery were manufactured in the same manner as in Example 1, except that natural graphite particles were heat-treated in an air atmosphere at 600°C for 1 hour in a continuous rotary kiln.
[0160]
[0161] Example 3
[0162] In the carbon-based active material preparation step, a negative electrode active material and a lithium secondary battery were manufactured in the same manner as in Example 1, except that natural graphite particles were heat-treated in an air atmosphere at 600°C for 5 hours in a continuous rotary kiln.
[0163]
[0164] Comparative Example 1
[0165] In the carbon-based active material preparation step, a negative active material and a lithium secondary battery were manufactured in the same manner as in Example 1, except that a low-crystalline carbon material was coated instead of oxidizing natural graphite particles. The coating treatment was specifically performed using the following method.
[0166] Natural graphite particles and petroleum pitch were mixed in a weight ratio of 100:5, mechanically mixed in a high-speed stirrer at 2000 rpm for 10 minutes to form a uniform mixture, heat-treated at 1200°C for 5 hours under a nitrogen atmosphere, and then classified through a 75 μm sieve.
[0167]
[0168] Comparative Example 2
[0169] In the carbon-based active material preparation step, a negative electrode active material and a lithium secondary battery were manufactured in the same manner as in Example 1, except that instead of oxidizing the natural graphite particles, natural graphite particles and petroleum pitch were mixed in a weight ratio of 100:8 and then heat-treated.
[0170]
[0171] Comparative Example 3
[0172] In the carbon-based active material preparation step, a negative electrode active material and a lithium secondary battery were manufactured in the same manner as in Example 1, except that the natural graphite particles were not subjected to oxidation treatment.
[0173]
[0174] Comparative Example 4
[0175] In the silicon-based active material preparation step, a negative electrode active material and a lithium secondary battery were manufactured in the same manner as in Example 1, except that the second grinding was applied only once.
[0176]
[0177] Experimental Example 1: Evaluation of Active Material Properties
[0178] The properties of the negative active materials manufactured according to the examples and comparative examples were evaluated, and the results are shown in Tables 1 to 2 and Fig. 2 below. The specific experimental methods are as follows.
[0179] (1) Evaluation of sphericity of carbon-based active materials
[0180] The sphericity of carbon-based active material powders was evaluated by dividing the perimeter of a circle with the same area as the particle projection shape by the actual perimeter of the particle projection shape using a flow particle analysis device. This sphericity can be measured using an analyzer for optical image acquisition (Fluid Imaging Technologies, Flowcam 8100) and analysis software (visual spreadsheet).
[0181] (2) Evaluation of circularity of silicon-based active materials
[0182] The circularity of the silicon-based active material powder was evaluated by dividing the perimeter of each particle by the perimeter of a circle with an equivalent area using an image analysis device. This circularity can be measured using an optical image acquisition analyzer (Malvernpanalytical, Morphholgi 4).
[0183] (3) Evaluation of silicon-based active material crystal grain size and strain
[0184] XRD data of silicon-based active materials were measured using Bruker's D8 Discover with GADDS XRD equipment, and crystal size and microstrain were measured using the Reitveld refinement method built into Bruker's DIFFRAC.TOPAS program.
[0185] (4) Evaluation of active material (mixture) tap density
[0186] Based on ASTM-B527, 10 g of active material powder was placed in a 50 mL container and tapped at 3000 cycles @ 284 cycles / min to measure the packing density.
[0187] (5) Evaluation of shrinkage density of active material (mixture)
[0188] 2 cm in diameter 22g of active material powder was injected into the circular mold and 700 kgf / cm 2 , 800 kgf / cm 2 , 900 kgf / cm 2 , 1000 kgf / cm 2 , 1200 kgf / cm 2 , 1300 kgf / cm 2 After applying compression pressure, the density was measured to determine the pellet density. Afterwards, the difference between the measured pellet density and the tap density was calculated to derive the shrinkage density.
[0189] (5) Evaluation of particle size of active material (mixture)
[0190] For the active material powder, measurements were made using the laser diffraction method.
[0191] At this time, particle size (D10), particle size (D50), particle size (D90) and particle size (Dmax) mean particle sizes corresponding to 10%, 50%, 90% and 100% of the volume accumulation amount in the particle size distribution curve, respectively, and SPAN means (particle size (D90) - particle size (D10)) / particle size (D50).
[0192] (6) Evaluation of the specific surface area of active material (mixture)
[0193] The specific surface area was measured using the BET method (Surface area and Porosity analyzer) (Micromeritics, ASAP2020).
[0194] Types of carbon-based active materials Surface treatment characteristics Carbon-based active material sphericity Silicon-based active material Types of silicon-based active materials Circularity of silicon-based active materials Crystalline size (nm) Silicon-based active material strain (×10 -5 ) Active material tap density (g / cm) 3)Example 1 Oxidation treatment Natural graphite oxidation 3 hours 0.88 Silicon 0.93 116 8 10.5 0.89Example 2 Oxidation treatment Natural graphite oxidation 1 hour 0.89 Silicon 0.93 116 8 10.5 0.89Example 3 Oxidation treatment Natural graphite oxidation 5 hours 0.87 Silicon 0.93 116 8 10.5 0.89Comparative Example 1 Coating treatment Natural graphite coating 3% 0.87 Silicon 0.93 116 8 10.5 1.10Comparative Example 2 Coating 5% 0.88 Silicon 0.93 116 8 10.5 1.05Comparative Example 3 Natural graphite uncoated 0.91 Silicon 0.93 116 8 10.5 0.97Comparative Example 4 Oxidation treatment Natural graphite oxidation 3 hours 0.88 silicon 0.93 180 90.93
[0195] Shrinkage density according to compression pressureCompression pressure (kg / cm) 2 )700800900100012001300Example 10.890.930.971.001.061.09Example 20.810.850.890.920.981.01Example 30.991.031.071.101.161.19Comparative Example 10.410.460.510.540.620.65Comparative Example 20.340.390.440.470.550.58Comparative Example 30.510.560.610.640.720.75Comparative Example 40.610.640.660.700.750.78
[0196] D10(μm)D50(μm)D90(μm)Dmax(μm)SPANSpecific surface area(m) 2 / g)Example 19.618.031.273.41.204.95Example 29.517.829.062.01.104.10Example 39.818.232.174.01.234.45Comparative Example 110.418.127.661.70.951.68Comparative Example 210.819.028.662.00.941.81Comparative Example 39.418.429.752.01.14.41Comparative Example 49.718.232741.234.96
[0197]
[0198] Referring to Tables 1 to 3 and FIG. 2, in the case of Examples 1 to 3, oxidized graphite was used as the carbon-based active material, and silicon particles with appropriately controlled circularity, grain size, and strain through first, second, and third pulverization were used as the silicon-based active material, and it was confirmed that the shrinkage density was properly implemented within the target range. On the other hand, in the case of Comparative Examples 1 to 3, which used coated or uncoated natural graphite rather than oxidized natural graphite as the carbon-based active material, it was confirmed that the shrinkage density was too low.
[0199] In addition, in the case of Comparative Example 4, which was performed only once during the second silicon pulverization process, it was confirmed that the circularity of the silicon was small, the crystal grain size was large, and the shrinkage density was too small as the strain was small.
[0200]
[0201] Experimental Example 2: Evaluation of Cathode Volume Expansion Rate
[0202] The volume expansion rate of the negative electrode was evaluated after 30 cycles of charge and discharge in lithium secondary batteries manufactured according to the examples and comparative examples, and the results are shown in Table 4 below.
[0203] More specifically, the thickness of the negative electrode manufactured according to the Examples and Comparative Examples was measured, and after manufacturing a half cell of a lithium secondary battery CR2032, a charge / discharge test was performed after aging at 25℃ for 30 hours. In order to evaluate the expansion characteristics, 500 mAh / g was used as the reference capacity, and the battery was charged to 5 mV at a constant current of 0.5 C, then switched to a constant voltage and charged until the end current reached 0.005 C. After a rest time of 10 minutes after charging, 30 cycles of discharge were performed at a constant current of 0.5 C with a reference capacity of 500 mAh / g until the battery reached 1.2 V. Afterwards, the battery was charged again to 5 mV at a constant current of 0.5 C, then switched to a constant voltage and charged until the end current reached 0.005 C, the battery was disassembled, and the electrode was washed with a DMC solvent for 5 minutes. The electrode thickness was measured, and the negative electrode thickness expansion rate was calculated using the following formula.
[0204] <Formula 1>
[0205] Volume expansion ratio (%) = (electrode thickness disassembled after 30 cycles - electrode thickness before assembly) / (electrode thickness before assembly) X 100
[0206] Volume expansion ratio (%) Example 141.6 Example 242.5 Example 338.4 Comparative Example 146.8 Comparative Example 250.6 Comparative Example 344.9 Comparative Example 443.8
[0207]
[0208] Referring to Table 4, it was confirmed that the volume expansion rate was significantly reduced in Examples 1 to 3 compared to Comparative Examples 1 to 4. This can be interpreted as a result of the shrinkage density of the negative electrode active material being controlled within an appropriate range.
[0209]
[0210] Experimental Example 3: Evaluation of Battery Electrochemical Characteristics
[0211] The electrochemical characteristics of lithium secondary batteries manufactured according to the examples and comparative examples were evaluated, and the results are shown in Table 5 and Fig. 3 below. The specific experimental methods are as follows.
[0212] (1) Evaluation of initial discharge capacity and initial efficiency
[0213] After fabricating a half-cell of a lithium secondary battery CR2032, we aged it at 25°C for 30 hours and then performed a charge-discharge test. To evaluate the initial capacity, we used 500 mAh / g as the reference capacity and charged it at a constant current of 0.1 C to 5 mV. Then, we switched to a constant voltage and charged it until the end current reached 0.005 C. After a 10-minute rest period after charging, we discharged it at a constant current of 0.1 C, using 500 mAh / g as the reference capacity, until it reached 1.0 V.
[0214] (2) Life characteristics evaluation
[0215] The life characteristics were measured by charging the battery to 5 mV at a constant current of 0.5 C at 25°C, then switching to a constant voltage and charging until the end current reached 0.005 C. After a 10-minute rest period after charging, the battery was discharged at a constant current of 0.5 C until the voltage reached 1.2 V. Thirty charge / discharge cycles were performed under these charge / discharge conditions, and the capacity retention rate of the 30th cycle was calculated compared to the first cycle.
[0216] Initial discharge capacity (mAh / g) Initial efficiency (%) Life characteristics (30 cycles, %) Example 1498.890.178.8 Example 2498.790.074.8 Example 3489.789.281.8 Comparative example 1479.387.565.5 Comparative example 2469.184.263.0 Comparative example 3485.287.367.8 Comparative example 4495.590.068.5
[0217] Referring to Table 5, it was confirmed that the capacity and life characteristics of the batteries of Examples 1 to 3 were significantly improved compared to Comparative Examples 1 to 4. This can be interpreted as a result of the shrinkage density of the negative electrode active material being controlled within an appropriate range.
[0218] Although the preferred embodiments of the present invention have been described above, the present invention is not limited thereto, and various modifications can be made within the scope of the patent claims, the detailed description of the invention, and the attached drawings, and it is obvious that this also falls within the scope of the present invention.
[0219] Accordingly, the actual scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. Contains a mixture of carbon-based active materials and silicon-based active materials, 700 to 1300 kgf / cm 2 Shrinkage density at compression pressures in the range of 0.80 g / cm 3 The above shrinkage density is defined as the difference between the pellet density and the tap density. Negative active material for lithium secondary batteries.
2. In paragraph 1, 1000 kgf / cm 2 At a compression pressure of 0.90 g / cm, the shrinkage density is 3 A negative electrode active material for a lithium secondary battery.
3. In paragraph 1, 1300 kgf / cm 2 Shrinkage density at a compression pressure of 1.00 g / cm 3 A negative electrode active material for a lithium secondary battery.
4. In paragraph 1, The above carbon-based active material is a negative electrode active material for a lithium secondary battery, which is natural graphite.
5. In paragraph 1, A negative active material for a lithium secondary battery, wherein the sphericity of the above carbon-based active material is 0.87 or higher.
6. In paragraph 1, The above carbon-based active material is an oxidized negative active material for a lithium secondary battery.
7. In paragraph 1, The above silicon-based active material is a negative electrode active material for a lithium secondary battery, which is a silicon particle.
8. In paragraph 1, The above silicon-based active material is a negative electrode active material for a lithium secondary battery having a circularity of 0.931 or more.
9. In paragraph 1, The above silicon-based active material is a negative electrode active material for a lithium secondary battery having a crystal grain size of 175 nm or less.
10. In paragraph 1, The above silicon-based active material has a strain of 10×10 -5 A negative electrode active material for a lithium secondary battery.
11. In paragraph 1, A negative electrode active material for a lithium secondary battery, wherein the content of the above silicon-based active material is 4 to 6 wt% based on the total weight of the mixture.
12. Step of preparing carbon-based active material; A step of preparing a silicon-based active material by sequentially performing a first crushing, a second crushing, and a third crushing of silicon-based active material raw materials; and A method for manufacturing a negative electrode active material, comprising a step of forming a mixture by mixing the above carbon-based active material and the above silicon-based active material, The above negative active material has a density of 700 to 1300 kgf / cm 2 Shrinkage density at compression pressures in the range of 0.80 g / cm 3 The above shrinkage density is defined as the difference between the pellet density and the tap density. A method for manufacturing a negative electrode active material for a lithium secondary battery.
13. In paragraph 12, In the step of preparing the above carbon-based active material, The above carbon-based active material is a method for manufacturing a negative electrode active material for a lithium secondary battery, wherein the negative electrode active material is natural graphite.
14. In paragraph 12, In the step of preparing the above carbon-based active material, The above carbon-based active material is a method for manufacturing a negative electrode active material for a lithium secondary battery having a sphericity of 0.87 or higher.
15. In paragraph 12, After the step of preparing the above carbon-based active material, A method for manufacturing a negative electrode active material for a lithium secondary battery, further comprising a step of performing oxidation treatment by heat treatment on the prepared carbon-based active material under an air atmosphere.
16. In paragraph 16, A method for manufacturing a negative electrode active material for a lithium secondary battery, wherein the above heat treatment is performed at a temperature of 500 to 700°C.
17. In paragraph 16, A method for manufacturing a negative electrode active material for a lithium secondary battery, wherein the above heat treatment is performed for 1 to 5 hours.
18. In paragraph 12, In the step of forming the above mixture, A method for producing a negative electrode active material for a lithium secondary battery, wherein the content of the above silicon-based active material is 4 to 6 wt% based on the total weight of the mixture.
19. A lithium secondary battery comprising a positive electrode; a negative electrode; an electrolyte; and a separator, wherein the negative electrode comprises the negative electrode active material of any one of claims 1 to 11.
Citation Information
Patent Citations
Negative electrode active material for nonaqueous electrolyte secondary battery, method for manufacturing negative electrode active material for nonaqueous electrolyte secondary battery, and negative electrode material for nonaqueous electrolyte secondary battery
JP2017062974A
Electro active material for secondary battery, conductive composition for secondary battery, cathode material, cathode structure and secondary battery comprising the same, and fabricating methods thereof
KR1020180117583A
Target object adaptive depth variable augmented reality apparatus and method
KR1020230167578A
Method and apparatus for compensating color separation of image in laser projector based holographic HUD
KR102791936B1