Thermoformable film and manufacturing method thereof
Patent Information
- Application Number
- PCT/KR2024/006625
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-16
- Filing Date
- 2024-05-16
- Publication Date
- 2024-11-21
AI Technical Summary
Conventional thermoformable films used in retort food manufacturing lose gas barrier properties during the thermoforming and heat sterilization processes, which can affect the quality of the contents, especially those sensitive to heat and gas permeation.
A thermoformable film comprising a first unstretched film layer, a stretched film layer with a transparent vapor deposition layer, and a second unstretched film layer, specifically designed to maintain gas barrier properties and thermoformability even after thermoforming and heat sterilization, with optimized tensile strength, elongation, and permeability characteristics.
The film ensures excellent gas barrier properties and heat resistance, preventing adverse effects on the contents during long-term storage and extending the shelf life of packaged items, particularly processed meat products.
Smart Images

Figure KR2024006625_21112024_PF_FP_ABST
Abstract
Description
Thermoformable film and method for producing the same
[0001] The present invention relates to a thermoformable film having excellent gas barrier properties and thus capable of improving the long-term storage properties of contents (e.g., food), and a method for producing the same.
[0002] Thermoformable films are used in the manufacture of retort foods, such as meat products, which are sealed. These thermoformable films must possess heat resistance to withstand heat sterilization processes and gas barrier properties to block oxygen and / or moisture, enabling long-term storage of the contents.
[0003] Conventionally, retort foods have been manufactured using coextruded films with excellent thermoformability as the thermoformable film. Specifically, the coextruded film is placed on a mold within a chamber, heated, and a vacuum is applied to thermoform the coextruded film to the mold shape. The contents are then added and sealed. The sealed contents are then heat-sterilized to produce the retort food.
[0004] However, since the co-extruded film has a structure in which films of the same thickness are combined (e.g., a structure in which two polypropylene films are combined), the thickness becomes very thin during the process of stretching it to fit the mold shape (thermoforming), resulting in poor gas barrier properties. If heat sterilization of the contents is performed in this state of poor gas barrier properties, the contents may be adversely affected. Specifically, if the contents are sensitive to heat treatment conditions or gas permeability, the color of the contents may change.
[0005] Therefore, there is a need to develop a thermoformable film that exhibits excellent gas barrier properties and a required level of thermoformability even after undergoing thermoforming and heat sterilization processes.
[0006] [Prior Art Literature]
[0007] [Patent Document]
[0008] (Patent Document 1) Republic of Korea Publication Patent No. 2010-0085157
[0009] The present invention aims to provide a thermoformable film that has thermoformability, heat resistance, etc. required in a thermoforming process and a heat sterilization process, and can exhibit excellent gas barrier properties even after these processes.
[0010] In addition, the present invention aims to provide a method for manufacturing a thermoformable film capable of efficiently manufacturing the thermoformable film.
[0011] In order to solve the above problem, according to one aspect of the present invention, a thermoformable film is provided, which includes a first non-stretched film layer; a stretched film layer including a transparent deposition layer formed on one or both sides; and a second non-stretched film layer.
[0012] In one embodiment, the thermoformable film may have an oxygen permeability (OTR) of 20 cc / ㎡·day or less, measured after thermoforming at 120 to 155°C.
[0013] In another embodiment, the thermoformable film may have an oxygen permeability (OTR) of 15 cc / ㎡·day or less, measured after heating the thermoformed film at 110 to 130°C for 20 to 30 minutes.
[0014] In another embodiment, the first non-stretchy film layer may have a tensile strength in the longitudinal direction (MD) and the transverse direction (TD) of 110 to 160 MPa, and an elongation in the longitudinal direction (MD) and the transverse direction (TD) of 400 to 440%, respectively.
[0015] In another embodiment, the stretched film layer may have a tensile strength in the longitudinal direction (MD) and the transverse direction (TD) of 240 to 320 MPa, and an elongation in the longitudinal direction (MD) and the transverse direction (TD) of 80 to 120%, respectively.
[0016] In another embodiment, the first non-stretchy film layer may have an oxygen permeability (OTR) of 30 cc / ㎡·day or less and a moisture vapor transmission rate (WVTR) of 250 g / ㎡·day or less.
[0017] In another embodiment, the stretched film layer may have an oxygen permeability (OTR) of 2 cc / ㎡·day or less and a moisture vapor transmission rate (WVTR) of 3 g / ㎡·day or less.
[0018] In another embodiment, the first non-stretched film layer and the stretched film layer may each include polyamide, and the second non-stretched film layer may include polypropylene.
[0019] In another embodiment, the sum of the thickness of the first non-stretched film layer and the thickness of the stretched film layer may be less than the thickness of the second non-stretched film layer.
[0020] In another embodiment, the thickness of the first non-stretched film layer may be 40 to 60 μm, the thickness of the stretched film layer may be 5 to 25 μm, and the thickness of the second non-stretched film layer may be 80 to 120 μm.
[0021] In another embodiment, the first non-stretched film layer, the stretched film layer, and the second non-stretched film layer may be sequentially laminated.
[0022] In another embodiment, the transparent deposition layer may include at least one selected from the group consisting of aluminum oxide, aluminum oxynitride, titanium oxide, silicon oxide, zinc oxide, tin oxide, silicon nitride, aluminum nitride, silicon oxynitride, nickel oxide, and magnesium oxide.
[0023] According to another aspect of the present invention, a method for manufacturing a thermoformable film is provided, comprising the steps of preparing a first unstretched film, a stretched film, and a second unstretched film, respectively; and the steps of sequentially laminating and bonding the first unstretched film, the stretched film, and the second unstretched film.
[0024] According to another aspect of the present invention, a retort pouch comprising the thermoformable film is provided.
[0025] The thermoformable film according to the present invention comprises a stretched film layer having gas barrier properties and thermoformability, and first and second non-stretched film layers capable of increasing thermoformability, so that it can exhibit thermoformability at a required level and can exhibit excellent heat resistance, sealing properties, gas barrier properties, etc. even after undergoing both the thermoforming process and the heat sterilization process.
[0026] Therefore, when using the thermoformable film according to the present invention to package various items such as food, pharmaceuticals, cosmetics, and industrial products, the long-term storage properties of the contents can be improved. In particular, the thermoformable film according to the present invention exhibits excellent gas barrier properties even when heat sterilization is performed under harsher conditions than boiling water sterilization, and thus can be usefully used in the manufacture of retort pouches used to ensure the long-term shelf life of processed meat products.
[0027] FIG. 1 is a cross-sectional view illustrating a thermoformable film according to one embodiment of the present invention.
[0028] Figure 2 is a flow chart showing a process for manufacturing a thermoformable film according to one embodiment of the present invention.
[0029] Hereinafter, the present invention will be described through examples. Herein, the present invention is not limited to the contents disclosed below, and may be modified in various forms without changing the gist of the invention.
[0030] Any reference herein to one component being formed above or below another component, or to being connected or joined to one another, encompasses both direct formation, connection, or joining between these components or indirect formation, connection, or joining through the interposition of another component. It should also be understood that the criteria for the upper / lower position of each component may vary depending on the direction from which the object is observed.
[0031] The word "comprising" or "including" in this specification is intended to specify particular features, regions, steps, processes, elements and / or components, and does not exclude the presence or addition of other features, regions, steps, processes, elements and / or components, unless specifically stated to the contrary.
[0032] All numbers and expressions indicating the amounts of components, reaction conditions, etc. described in this specification can be understood to be modified by the term “about” in all cases unless otherwise specified.
[0033] In this specification, terms such as first, second, etc. are used to describe various components, and the components are not limited by the terms. Specifically, the terms are used to distinguish one component from another.
[0034]
[0035] thermoformable film
[0036] The present invention provides a thermoformable film that has superior gas barrier properties compared to conventional coextruded films and ensures thermoformability (stretchability). Specifically, the thermoformable film according to the present invention comprises a first non-stretched film layer; a stretched film layer; and a second non-stretched film layer, which will be described in detail with reference to FIG. 1 as follows.
[0037]
[0038] First non-stretched film layer
[0039] The first non-stretched film layer (10) included in the thermoformable film (100) according to the present invention serves to secure heat resistance, pinhole resistance, gas barrier properties, etc. of the thermoformable film (100). This first non-stretched film layer (10) may be formed of a film containing a polymer resin (first polymer resin), and in this case, the film may be an unstretched film. The polymer resin (first polymer resin) is not particularly limited, but may specifically include polyamide. Since the first non-stretched film layer (10) contains the polyamide, the pinhole resistance, gas barrier properties, and mechanical strength of the thermoformable film (100) can be increased. The above polyamide may be specifically at least one selected from the group consisting of nylon 4, nylon 6, nylon 7, nylon 8, nylon 11, nylon 12, nylon 66, nylon 69, nylon 610, nylon 611, nylon 612, nylon 6T, nylon 6 / 66, nylon 6 / 12, nylon 6 / 6T, nylon 6T (terephthalic acid) / 6I (isophthalic acid), and nylon MXD6.
[0040] According to the present invention, the first non-stretchy film layer (10) can exhibit mechanical (physical) properties (e.g., tensile strength, elongation, etc.) controlled within a specific range, thereby ensuring the gas barrier properties of the thermoformable film (100) while increasing the thermoformability (stretchability).
[0041] Specifically, the first non-stretched film layer (10) may have a tensile strength in the longitudinal direction (MD) and the transverse direction (TD) of 110 to 160 MPa, respectively. For example, the first non-stretched film layer (10) may have a tensile strength in the longitudinal direction (MD) of 115 to 160 MPa, 120 to 155 MPa, 125 to 155 MPa, 130 to 150 MPa, 135 to 150 MPa, or 135 to 145 MPa. In addition, the first non-stretched film layer (10) may have a tensile strength in the transverse direction (TD) of 110 to 155 MPa, 115 to 150 MPa, 115 to 145 MPa, 120 to 140 MPa, 125 to 135 MPa, or 125 to 130 MPa. Here, the tensile strength (A) of the first non-stretched film layer (10) in the longitudinal direction (MD) may be greater than the tensile strength (B) in the transverse direction (TD) (A>B). The tensile strength of the first non-stretched film layer (10) may be measured according to the JIS K 7127 standard (@23 ℃).
[0042] The first non-stretched film layer (10) may have an elongation in the longitudinal direction (MD) and the transverse direction (TD) of 400 to 440%, respectively. For example, the first non-stretched film layer (10) may have an elongation in the longitudinal direction (MD) of 400 to 435%, 403 to 430%, 405 to 425%, 407 to 420%, or 409 to 415%. In addition, the first non-stretched film layer (10) may have an elongation in the transverse direction (TD) of 405 to 440%, 410 to 438%, 415 to 435%, 420 to 435%, or 425 to 433%. Here, the elongation (C) in the longitudinal direction (MD) of the first non-stretch film layer (10) may be smaller than the elongation (D) in the transverse direction (TD) (C <D). 이러한 제1 무연신 필름층(10)의 신율은 JIS K 7127 규격(@23℃)에 의거하여 측정할 수 있다.
[0043] Meanwhile, the first non-stretched film layer (10) may have a tear strength in the longitudinal direction (MD) and the transverse direction (TD) of 130 to 220 N / cm, respectively. For example, the first non-stretched film layer (10) may have a tear strength in the longitudinal direction (MD) of 130 to 210 N / cm, 135 to 200 N / cm, 135 to 190 N / cm, 140 to 180 N / cm, 140 to 170 N / cm, or 145 to 155 N / cm. In addition, the first non-stretched film layer (10) may have a tear strength in the width direction (TD) of 145 to 220 N / cm, 155 to 215 N / cm, 170 to 215 N / cm, 185 to 210 N / cm, or 195 to 205 N / cm. Here, the tear strength (E) in the length direction (MD) of the first non-stretched film layer (10) may be smaller than the tear strength (F) in the width direction (TD) (E <F). 이러한 제1 무연신 필름층(10)의 인열강도는 JIS K 7128 규격(@23℃)에 의거하여 측정할 수 있다.
[0044] In addition, the first non-stretched film layer (10) may have a haze of 4% or less, 3.9% or less, 3.8% or less, 3.7% or less, 3.6% or less, or 3.5% or less. The haze of the first non-stretched film layer (10) may be measured according to the JIS K 7105 standard (@23°C).
[0045] According to the present invention, the first non-stretched film layer (10) may have an oxygen permeability (OTR) of 30 cc / m2·day or less (= 30 cc / m2·day·atm or less) and a water vapor permeability (WVTR) of 250 g / m2·day or less. Specifically, the first non-stretched film layer (10) may have an oxygen permeability (OTR) of 25 cc / m2·day or less, 20 cc / m2·day or less, 15 cc / m2·day or less, 10 cc / m2·day or less, or 5 cc / m2·day or less, and may be 0 cc / m2·day or more, 0.0001 cc / m2·day or more, 0.0002 cc / m2·day or more, 0.0003 cc / m2·day or more, or 0.0004 cc / m2·day or more. In addition, the first non-stretch film layer (10) may have a water vapor transmission rate (WVTR) of 230 g / m2·day or less, 200 g / m2·day or less, 180 g / m2·day or less, 165 g / m2·day or less, or 150 g / m2·day or less, or 0.00001 g / m2·day or more, 0.00003 g / m2·day or more, 0.00005 g / m2·day or more, 0.0001 g / m2·day or more, or 0.0005 g / m2·day or more. Since the oxygen permeability (OTR) and moisture permeability (WVTR) of the first non-stretched film layer (10) are within the above ranges, the gas barrier property of the thermoformable film (100) can be increased while the heat resistance, pinhole resistance, etc. of the thermoformable film (100) can be secured, thereby significantly increasing the long-term storage property of the retort pouch manufactured using the thermoformable film (100). The oxygen permeability (OTR) of the first non-stretched film layer (10) can be measured according to the JIS K 7126 standard (@23℃×0%RH), and the moisture permeability (WVTR) of the first non-stretched film layer (10) can be measured according to the JIS K 7129 standard (@40℃×90%RH).
[0046] According to the present invention, the first non-stretched film layer (10) may have a thickness of 40 to 60 μm. Specifically, the first non-stretched film layer (10) may have a thickness of 43 to 58 μm, 45 to 55 μm, 48 to 53 μm, or 49 to 51 μm. When the thickness of the first non-stretched film layer (10) is within the above range, the gas barrier properties and thermoformability of the thermoformable film (100) can be improved.
[0047]
[0048] Stretch film layer
[0049] The stretched film layer (20) included in the thermoformable film (100) according to the present invention serves to increase the heat resistance, durability, gas barrier properties, thermoformability, etc. of the thermoformable film (100). This stretched film layer (20) may be formed of a film obtained by uniaxially or biaxially stretching a non-stretched film containing a polymer resin (second polymer resin). The polymer resin (second polymer resin) is not particularly limited, but may specifically include polyamide. Since the stretched film layer (20) includes the polyamide, the gas barrier properties, mechanical strength, and thermoformability of the thermoformable film (100) can be increased. The above polyamide may be specifically at least one selected from the group consisting of nylon 4, nylon 6, nylon 7, nylon 8, nylon 11, nylon 12, nylon 66, nylon 69, nylon 610, nylon 611, nylon 612, nylon 6T, nylon 6 / 66, nylon 6 / 12, nylon 6 / 6T, nylon 6T (terephthalic acid) / 6I (isophthalic acid), and nylon MXD6.
[0050] The above-described stretched film layer (20) may include a transparent deposition layer (not shown) formed on one or both sides thereof. Since the stretched film layer (20) includes the transparent deposition layer, a thermoformable film (100) having transparency while increasing the gas barrier properties and mechanical strength of the thermoformable film (100) can be provided. Therefore, when a retort pouch is manufactured using the thermoformable film (100) according to the present invention, a retort pouch having significantly increased long-term storage properties of the contents while allowing confirmation of the contents can be provided. This transparent deposition layer may be formed on one side of the stretched film layer (20), and the stretched film layer (20) and the second non-stretched film layer (30) may be arranged (combined) so that the second non-stretched film layer (30) described below and the transparent deposition layer face each other.
[0051] According to the present invention, the transparent deposition layer may include an inorganic material having transparency and excellent gas barrier properties. Specifically, the transparent deposition layer may include aluminum oxide (AlO x ), aluminum oxynitride (AlO x N y ), titanium oxide (TiO x ), silicon oxide (SiO x ), zinc oxide (ZnO x ), tin oxide (SnO x ), silicon nitride (SiN x ), aluminum nitride (AlN) x ), silicon nitride (SiO x N y ), nickel oxide (NiO x ) and magnesium oxide (MgO x ) may include one or more selected from the group consisting of.
[0052] This transparent deposition layer may have a thickness of 5 to 50 nm. Specifically, the thickness of the transparent deposition layer may be 7 to 40 nm, 9 to 35 nm, 10 to 30 nm, or 10 to 25 nm. As the thickness of the transparent deposition layer is within the above range, the gas barrier property of the thermoformable film (100) can be increased while preventing the stretchable film layer (20) from being deformed by the transparent deposition layer.
[0053] According to the present invention, the stretchable film layer (20) including the transparent deposition layer can exhibit mechanical (physical) properties (e.g., tensile strength, elongation, etc.) controlled within a specific range, thereby increasing the gas barrier properties and thermoformability (stretchability) of the thermoformable film (100).
[0054] Specifically, the stretched film layer (20) may have a tensile strength in the longitudinal direction (MD) and the transverse direction (TD) of 240 to 320 MPa, respectively. For example, the stretched film layer (20) may have a tensile strength in the longitudinal direction (MD) of 240 to 310 MPa, 245 to 300 MPa, 250 to 290 MPa, 250 to 280 MPa, 255 to 270 MPa, or 255 to 265 MPa. In addition, the stretched film layer (20) may have a tensile strength in the transverse direction (TD) of 250 to 320 MPa, 260 to 315 MPa, 270 to 315 MPa, 280 to 310 MPa, 290 to 305 MPa, or 295 to 305 MPa. Here, the tensile strength (a) in the longitudinal direction (MD) of the stretched film layer (20) may be less than the tensile strength (b) in the transverse direction (TD) (a <b). 이러한 연신 필름층(20)의 인장강도는 JIS K 7127 규격(@23 ℃)에 의거하여 측정할 수 있다.
[0055] The stretched film layer (20) may have an elongation in the longitudinal direction (MD) and the transverse direction (TD) of 80 to 120%, respectively. For example, the stretched film layer (20) may have an elongation in the longitudinal direction (MD) of 85 to 120%, 90 to 118%, 95 to 115%, 100 to 113%, or 105 to 112%. In addition, the stretched film layer (20) may have an elongation in the transverse direction (TD) of 80 to 110%, 82 to 105%, 84 to 100%, 86 to 95%, or 88 to 93%. Here, the elongation (c) of the stretched film layer (20) in the longitudinal direction (MD) may be greater than the elongation (d) in the transverse direction (TD) (c>d). The elongation of this stretch film layer (20) can be measured according to the JIS K 7127 standard (@23℃).
[0056] Meanwhile, the above-mentioned stretched film layer (20) may have a total light transmittance of 85% or more, 86% or more, 87% or more, 88% or more, 89% or more, or 90% or more. The total light transmittance of the stretched film layer (20) may be measured according to the JIS K 7361-1 standard (@23°C).
[0057] In addition, the stretched film layer (20) may have a haze of 3.5% or less, 3.4% or less, 3.3% or less, 3.2% or less, 3.1% or less, or 3.0% or less. The haze of the stretched film layer (20) may be measured according to the JIS K 7136 standard (@23°C).
[0058] In addition, the stretched film layer (20) may have a shrinkage ratio in the longitudinal direction (MD) of 1.8% or less, 1.7% or less, 1.6% or less, or 1.5% or less (e.g., 1.3 to 1.6%), and a shrinkage ratio in the transverse direction (TD) of 2.3% or less, 2.2% or less, 2.1% or less, or 2.0% or less (e.g., 1.9 to 2.1%). The shrinkage ratio of the stretched film layer (20) may be calculated as a ratio (percentage) of the shrunken (reduced) length to the initial length after the stretched film is immersed in water at 95°C for 5 minutes.
[0059] According to the present invention, the stretched film layer (20) may have an oxygen permeability (OTR) of 2 cc / m2·day or less (= 2 cc / m2·day·atm or less) and a water vapor permeability (WVTR) of 3 g / m2·day or less. Specifically, the stretched film layer (20) may have an oxygen permeability (OTR) of 1.5 cc / m2·day or less, 1.3 cc / m2·day or less, 1.1 cc / m2·day or less, 0.8 cc / m2·day or less, or 0.6 cc / m2·day or less, and may have an OTR of 0 cc / m2·day or more, 0.0001 cc / m2·day or more, 0.0002 cc / m2·day or more, 0.0003 cc / m2·day or more, or 0.0004 cc / m2·day or more. In addition, the above-mentioned stretched film layer (20) may have a water vapor transmission rate (WVTR) of 2.5 g / m2·day or less, 2.0 g / m2·day or less, 1.5 g / m2·day or less, 1.1 g / m2·day or less, or 0.8 g / m2·day or less, or 0 g / m2·day or more, 0.00001 g / m2·day or more, 0.00005 g / m2·day or more, 0.0001 g / m2·day or more, 0.0003 g / m2·day or more, or 0.0005 g / m2·day or more. Since the oxygen permeability (OTR) and moisture permeability (WVTR) of the above-mentioned stretched film layer (20) are within the above-mentioned ranges, the gas barrier property of the thermoformable film (100) can be increased while the heat resistance, thermoformability, etc. of the thermoformable film (100) can be secured, and thus the formability and long-term storability of the retort pouch manufactured using the thermoformable film (100) can be significantly increased. The oxygen permeability (OTR) of the stretched film layer (20) can be measured according to the JIS K 7126 standard (@25℃×80%RH), and the moisture permeability (WVTR) of the stretched film layer (20) can be measured according to the JIS K 7129 standard (@40℃×90%RH).
[0060] According to the present invention, the stretched film layer (20) may have a thickness of 5 to 25 μm. Specifically, the stretched film layer (20) may have a thickness of 8 to 23 μm, 10 to 20 μm, 12 to 18 μm, or 14 to 16 μm. As the thickness of the stretched film layer (20) is within the above range, the gas barrier properties and thermoformability of the thermoformable film (100) can be improved.
[0061]
[0062] Second non-stretch film layer
[0063] The second non-stretched film layer (30) included in the thermoformable film (100) according to the present invention serves to secure heat resistance, moisture absorption resistance, sealing properties, thermoformability, etc. of the thermoformable film (100). This second non-stretched film layer (30) may be formed of a film including a polymer resin (third polymer resin), and at this time, the film may be an unstretched film. The polymer resin (third polymer resin) is not particularly limited, but may specifically include polypropylene. Since the second non-stretched film layer (30) includes the polymer resin, the heat resistance, sealing properties, and thermoformability of the thermoformable film (100) can be improved. For example, the second non-stretched film layer (30) may be formed of a non-stretched polypropylene film (CPP).
[0064] According to the present invention, the second non-stretched film layer (30) may have a thickness of 80 to 120 μm. Specifically, the second non-stretched film layer (30) may have a thickness of 83 to 118 μm, 85 to 115 μm, 90 to 110 μm, or 95 to 105 μm. As the thickness of the second non-stretched film layer (30) is within the above range, the sealing property and thermoformability of the thermoformable film (100) can be improved, while the overall thickness of the thermoformable film (100) can be prevented from becoming thicker than necessary.
[0065]
[0066] Meanwhile, according to the present invention, the first non-oriented film layer (10), the stretched film layer (20), and the second non-oriented film layer (30) described above can be sequentially laminated. Specifically, the thermoformable film (100) according to the present invention can have a structure in which the first non-oriented film layer (10) / the stretched film layer (the stretched polyamide substrate layer / the transparent deposition layer) (20) / the second non-oriented film layer (30) are laminated in this order, as illustrated in FIG. 1, and the thermoformability can be excellent due to this laminated structure. Here, in order to increase the bonding strength between each layer, an adhesive layer may be interposed between the first non-oriented film layer (10) and the stretched film layer (20) and / or between the stretched film layer (20) and the second non-oriented film layer (30).
[0067] The thermoformable film (100) according to the present invention may have a thickness (T1) of the first non-stretched film layer (10) and a thickness (T2) of the stretched film layer (20) in which the sum (T1+T2) of the thickness (T1) of the first non-stretched film layer (10) and the thickness (T2) of the stretched film layer (20) is smaller than the thickness (T3) of the second non-stretched film layer (30) (T1+T2) <T3). 이러한 두께 차를 나타낼 경우, 상기 열성형성 필름(100)을 몰드 모양에 맞춰 열성형하는 과정(연신시키는 과정)에서 열성형성 필름(100)의 두께가 과도하게 얇아지는 것이 방지되어 열성형이 이루어진 후에도 열성형성 필름(100)의 기체 차단성을 확보할 수 있다.
[0068] According to the present invention, the thickness ratio (T1:T2:T3) between the first non-stretched film layer (10), the stretched film layer (20), and the second non-stretched film layer (30) is not particularly limited, but may be 1:0.1 to 0.5:1.5 to 2.5, 1:0.2 to 0.4:1.7 to 2.3, or 1:0.2 to 0.3:1.8 to 2.1.
[0069] The thermoformable film (100) according to the present invention includes the stretched film layer (20) having high gas barrier properties and thermoformability (stretchability), and the first non-stretched film layer (10) and the second non-stretched film (30) having excellent thermoformability (stretchability), so that the gas barrier properties can be excellent even after the thermoforming process, or after the thermoforming process and the heat sterilization process. That is, the thermoformable film (100) according to the present invention can exhibit relatively low oxygen permeability (OTR) and moisture permeability (WVTR) even after undergoing the thermoforming process, or after undergoing both the thermoforming process and the heat sterilization process.
[0070] Specifically, according to the present invention, the thermoformable film (100) may have an oxygen permeability (OTR) measured after thermoforming at 120 to 155°C of 20 cc / ㎡·day or less (= 20 cc / ㎡·day·atm or less). More specifically, the thermoformable film (100) may have an oxygen permeability (OTR) after thermoforming of 15 cc / m2·day or less, 13 cc / m2·day or less, 10 cc / m2·day or less, 8 cc / m2·day or less, 5 cc / m2·day or less, or 1 cc / m2·day or less, or 0 cc / m2·day or more, 0.0001 cc / m2·day or more, 0.001 cc / m2·day or more, 0.01 cc / m2·day or more, 0.05 cc / m2·day or more, or 0.1 cc / m2·day or more. Here, the time for thermoforming the thermoformable film (100) at 120 to 155°C (specifically, 125 to 155°C, 130 to 155°C, or 135 to 155°C) is not particularly limited, but may be 3 to 15 seconds, 5 to 13 seconds, or 7 to 10 seconds. For example, the thermoforming of the thermoformable film (100) may be performed by heat treating at 120 to 155°C for 3 seconds and foaming for 5 seconds while maintaining the temperature at 120 to 155°C.
[0071] In addition, according to the present invention, the thermoformable film (100) may be thermoformed at 120 to 155°C and heated at 110 to 130°C for 20 to 30 minutes (after undergoing both the thermoforming and heat sterilization processes), and the measured oxygen permeability (OTR) may be 15 cc / ㎡·day or less (= 15 cc / ㎡·day·atm or less). More specifically, the thermoformable film (100) may have an oxygen permeability (OTR) after the thermoforming and heat treatment of 12 cc / m2·day or less, 9 cc / m2·day or less, 7 cc / m2·day or less, 5 cc / m2·day or less, or 3.5 cc / m2·day or less, and may be 0 cc / m2·day or more, 0.0001 cc / m2·day or more, 0.0002 cc / m2·day or more, 0.0003 cc / m2·day or more, 0.0004 cc / m2·day or more, or 0.0005 cc / m2·day or more. Here, the heating of the thermoformable film (100) in which thermoforming has been performed can be performed, for example, by storing it in steam at 110 to 130° C. or in hot water at 110 to 130° C. under a pressure higher than atmospheric pressure for 20 to 30 minutes.
[0072]
[0073] Method for manufacturing thermoformable film
[0074] The present invention provides a method for manufacturing a thermoformable film capable of efficiently manufacturing the thermoformable film described above. Specifically, the method for manufacturing a thermoformable film according to the present invention comprises the steps of respectively preparing a first unstretched film, a stretched film, and a second unstretched film; and the steps of sequentially laminating and bonding the first unstretched film, the stretched film, and the second unstretched film (see FIG. 2).
[0075] The step of preparing each of the above films may include a step of preparing a first unstretched film for forming the first unstretched film layer described above, a stretched film for forming the stretched film layer described above, and a second unstretched film for forming the second unstretched film layer described above, respectively.
[0076] The above first non-stretched film may be a non-stretched film including the above-described polymer resin (first polymer resin).
[0077] The above-mentioned stretched film may be a film that has undergone a deposition process after uniaxially or biaxially stretching a non-stretched film (second non-stretched film) containing the above-mentioned polymer resin (second polymer resin). Specifically, the stretched film may be a film that has undergone a deposition process after stretching the non-stretched film in at least one of the longitudinal direction (MD) and the transverse direction (TD). The deposition process may be a process of depositing an inorganic material having transparency and excellent gas barrier properties on the film that has undergone the stretching process. Here, the inorganic material may be aluminum oxide (AlO x ), aluminum oxynitride (AlO x N y ), titanium oxide (TiO x ), silicon oxide (SiO x ), zinc oxide (ZnO x ), tin oxide (SnO x ), silicon nitride (SiN x ), aluminum nitride (AlN) x ), silicon nitride (SiO x N y ), nickel oxide (NiO x ) and magnesium oxide (MgO x ) may include at least one selected from the group consisting of. In addition, the deposition process may be a commonly known deposition process (e.g., sputter deposition; ion plating; or vacuum deposition using high-frequency heating, electron beam heating, etc.).
[0078] The second non-stretched film may be a non-stretched film comprising the polymer resin described above (third polymer resin). Specifically, the second non-stretched film may be a non-stretched polypropylene film (CPP).
[0079]
[0080] The step of combining the respective films may include a step of sequentially laminating the first unstretched film, the stretched film, and the second unstretched film, and combining them using a commonly known lamination method. In addition, a step of applying an adhesive to one surface of at least one of the first unstretched film, the stretched film, and the second unstretched film before laminating the respective films and sequentially laminating and combining the respective films may be included. The adhesive may be an adhesive commonly used in film manufacturing.
[0081]
[0082] retort pouch
[0083] The present invention provides a retort pouch comprising the thermoformable film described above. Specifically, the retort pouch according to the present invention is manufactured by laminating a top film and a bottom film and then performing a conventional sealing process, and at least one of the top film and the bottom film may be the thermoformable film described above. Since the retort pouch according to the present invention comprises the thermoformable film described above, it can be easily thermoformed into a desired shape, and can have excellent gas barrier properties even after thermoforming. In particular, the retort pouch according to the present invention exhibits excellent gas barrier properties even when heat sterilization is performed under harsher conditions than boiling water sterilization, thereby enabling an extension of the shelf life of the contents (e.g., processed meat products).
[0084] The retort pouch according to the present invention can have various types such as a box pouch, a three-way pouch, a T-way pouch, an M-way pouch, etc.
[0085]
[0086] The present invention is described in more detail through the following examples. However, the scope of the present invention is not limited to these examples.
[0087] <Manufacturing of thermoformable films>
[0088] Example 1
[0089] A polyamide film having a thickness of 50 μm was prepared as the first non-stretched film, a silicon dioxide-deposited polyamide film having a thickness of 15 μm was prepared as the stretched film, and a polypropylene film (CPP film) having a thickness of 100 μm was prepared as the second non-stretched film. The physical properties of each film are summarized in Table 1 below.
[0090] Next, a thermoformable film was manufactured by laminating a first non-stretched film layer (polyamide film layer) / stretched film layer (silicon dioxide-deposited polyamide film layer) / second non-stretched film layer (polypropylene film layer) in this order using a lamination method.
[0091]
[0092] Classification 1 Non-stretched filmStretched film Oxygen permeability (cc / ㎡ day) 20 or less 0.6 or less Moisture permeability (g / ㎡ day) 162 or less 0.8 or less Tensile strength (MPa) MD 140 260 TD 130 300 Elongation (%) MD 410 110 TD 430 90 Haze (%) 3.5 or less 3.0 or less
[0093] Comparative Example 1
[0094] A multilayer coextruded film (Xiangfu, 620C) manufactured using a non-stretch film was applied.
[0095]
[0096] <Manufacturing of Retort Pouches>
[0097] Manufacturing Example 1
[0098] A three-way type retort pouch was manufactured by laminating and sealing the thermoformable film of Example 1 as a top film and a bottom film, which are conventionally used in retort manufacturing.
[0099]
[0100] Comparative Manufacturing Example 1
[0101] A three-way type retort pouch was manufactured by laminating and sealing the co-extruded film of Comparative Example 1 as a top film and a bottom film, which are conventionally used in retort manufacturing.
[0102]
[0103] Test Example 1. Thermoformability Evaluation
[0104] Ham products were placed in the retort pouches manufactured in Manufacturing Example 1 and Comparative Manufacturing Example 1, respectively, and final sealing was performed to manufacture processed products. Afterwards, the presence of rounding (a phenomenon in which right-angle forming was not achieved) at the four corners of the processed products was visually checked, and the results are shown in Table 2 below.
[0105] ○: No corner rounding
[0106] △: Rounding on 1-2 of the four corners
[0107] ×: All four corners are rounded
[0108]
[0109] Test Example 2. Oxygen Permeability Measurement
[0110] The thermoformable films manufactured in Example 1 and Comparative Example 1 were each placed in a mold having a depth of 10 mm and thermoformed at 140 to 155°C for 8 seconds. Next, the thermoformed films were heat-sterilized at 118°C for 25 minutes. Thereafter, the oxygen permeability of the thermoformed and heat-sterilized films was measured using a Mocon Oxtran device according to the ASTM D3985 standard (@23°CХ50%RH), and the results are shown in Table 2 below.
[0111]
[0112] Classification Example 1 (Manufacturing Example 1) Comparative Example 1 (Comparative Manufacturing Example 1) Thermoforming △○ Oxygen permeability before thermoforming (cc / ㎡·day) 0.310 1.366 Oxygen permeability after thermoforming and heat sterilization (cc / ㎡·day) 3.36 21 8.924
[0113] Referring to Table 2 above, it can be confirmed that the thermoformable film according to the present invention has excellent gas barrier properties with significantly low oxygen permeability even after thermoforming and heat sterilization while ensuring thermoformability.
[0114] [Explanation of symbols]
[0115] 100: Thermoformable film
[0116] 10: First non-stretched film layer
[0117] 20: Stretch film layer
[0118] 30: Second non-stretch film layer
Claims
1. First non-stretch film layer; A stretched film layer comprising a transparent deposition layer formed on one or both sides; and A thermoformable film comprising a second non-stretch film layer.
2. In paragraph 1, A thermoformable film having an oxygen permeability (OTR) of 20 cc / ㎡·day or less, measured after thermoforming at 120 to 155°C.
3. In paragraph 2, A thermoformable film having an oxygen permeability (OTR) of 15 cc / ㎡·day or less, measured after heating the thermoformed film at 110 to 130°C for 20 to 30 minutes.
4. In paragraph 1, A thermoformable film, wherein the first non-stretched film layer has a tensile strength in the longitudinal direction (MD) and the transverse direction (TD) of 110 to 160 MPa, and an elongation in the longitudinal direction (MD) and the transverse direction (TD) of 400 to 440%, respectively.
5. In paragraph 1, A thermoformable film, wherein the above-mentioned stretched film layer has a tensile strength in the longitudinal direction (MD) and the transverse direction (TD) of 240 to 320 MPa, and an elongation in the longitudinal direction (MD) and the transverse direction (TD) of 80 to 120%, respectively.
6. In paragraph 1, A thermoformable film having an oxygen permeability (OTR) of 30 cc / ㎡·day or less and a moisture vapor permeability (WVTR) of 250 g / ㎡·day or less, wherein the first non-stretch film layer is a thermoformable film.
7. In paragraph 1, The above-mentioned stretch film layer is a thermoformable film having an oxygen permeability (OTR) of 2 cc / ㎡·day or less and a moisture vapor permeability (WVTR) of 3 g / ㎡·day or less.
8. In paragraph 1, The first non-stretched film layer and the stretched film layer each contain polyamide, A thermoformable film, wherein the second non-stretch film layer comprises polypropylene.
9. In paragraph 1, A thermoformable film, wherein the sum of the thickness of the first non-stretched film layer and the thickness of the stretched film layer is smaller than the thickness of the second non-stretched film layer.
10. In paragraph 1, The thickness of the first non-stretch film layer is 40 to 60 ㎛, The thickness of the above-mentioned stretched film layer is 5 to 25 ㎛, A thermoformable film, wherein the thickness of the second non-stretch film layer is 80 to 120 μm.
11. In paragraph 1, A thermoformable film in which the first non-stretched film layer, the stretched film layer, and the second non-stretched film layer are sequentially laminated.
12. In paragraph 1, A thermoformable film, wherein the transparent deposition layer comprises at least one selected from the group consisting of aluminum oxide, aluminum oxynitride, titanium oxide, silicon oxide, zinc oxide, tin oxide, silicon nitride, aluminum nitride, silicon oxynitride, nickel oxide, and magnesium oxide.
13. A step of preparing a first non-stretching film, a stretched film and a second non-stretching film, respectively; and A method for manufacturing a thermoformable film, comprising the step of sequentially laminating and bonding the first non-stretched film, the stretched film, and the second non-stretched film.
14. A retort pouch comprising a thermoformable film according to any one of claims 1 to 12.
Citation Information
Patent Citations
Structure of Packaging Material for Boil / Retort Sterilization and Method for Manufacturing Package Using the Packaging Material
JP6157973B2
Packaging Articles, Films and Methods that Promote or Preserve the Desirable Color of Meat
KR101274438B1
Composite sheet having excellent workability and preparing method for packing container comprising the same
KR102212094B1
Manufacturing method for food packaging
KR102299318B1
A method of manufacturing of instant rice packing materials using transparent deposition Nylon
KR102432490B1