Improved 3xx aluminum alloys and methods of making the same

WO2026212639A3PCT designated stage Publication Date: 2026-11-19ALCOA USA CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/US2025/028864
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-03-12
Filing Date
2025-05-12
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing aluminum alloys do not effectively balance strength, ductility, and bend angle properties, limiting their performance in various applications.

Method used

Development of 3xx aluminum casting alloys with specific compositions including Si, Mg, Mn, Cr, Fe, Cu, Zn, Ti, V, Zr, Sr, Sb, Na, and Ca, with balanced ranges to enhance strength, ductility, and bend angle properties, utilizing recycled aluminum sources and advanced casting processes.

Benefits of technology

The new alloys achieve improved mechanical properties, enabling enhanced performance in applications while promoting aluminum recycling and reducing environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure US2025028864_19112026_PF_FP_ABST
    Figure US2025028864_19112026_PF_FP_ABST
Patent Text Reader

Abstract

New 3xx aluminum casting alloys are described. The new 3xx aluminum casting alloys may include from 7.0 to 9.0 wt. % Si, from 0.05 to 0.6 wt. % Mg, from 0.1 to 0.4 wt. % Mn, from 0.05 to 0.25 wt. % Cr, wherein (wt. % Mn) + (wt. % Cr) is from 0.2 to 0.6 wt. %, from 0.05 to 1.5 wt. % Fe, up to 0.5 wt. % Cu, up to 0.5 wt. % Zn, up to 0.15 wt. % Ti, up to 0.15 wt. % V, up to 0.15 wt. % Zr, and up to 0.05 wt. % of any one of Sr, Sb, Na, and Ca, with the balance being aluminum, optional incidental elements and impurities. The aluminum casting alloys may be in a form of a shape cast product. Such shape cast products may realize an improved combination of properties.
Need to check novelty before this filing date? Find Prior Art

Description

Attorney Ref. No.: 169593.120026 / WOIMPROVED 3XX ALUMINUM ALLOYS AND METHODS OF MAKING THE SAMECROSS REFERENCE TO RELATED APPLICATION

[0001] This application claims priority to U.S. Provisional Patent Application No.63 / 770,516, entitled “3XX Aluminum Alloys and Methods of Making the Same,” filed March 12, 2025, which is hereby incorporated by reference in its entirety.BACKGROUND

[0002] Aluminum alloys are useful in a variety of applications. Some aluminum alloys are also recyclable, and recycling those aluminum alloys preserves energy resources. In the United States and Canada, more than 5 million tons of aluminum are recycled each year.SUMMARY OF THE DISCLOSURE

[0003] Broadly, the present patent application relates to new 3xx aluminum casting alloys having from 7.0 to 9.0 wt. % Si, from 0.05 to 0.6 wt. % Mg, from 0.1 to 0.4 wt. % Mn, from 0.05 to 0.25 wt. % Cr, wherein (wt. % Mn) + (wt. % Cr) is from 0.2 to 0.6 wt. %, from 0.05 to 1.5 wt. % Fe, up to 0.5 wt. % Cu, up to 0.5 wt. % Zn, up to 0.15 wt. % Ti, up to 0.15 wt. % V, up to 0.15 wt. % Zr, and up to 0.05 wt. % of any one of Sr, Sb, Na, and Ca, with the balance being aluminum, optional incidental elements, and impurities. The aluminum casting alloys may be in a form of an ingot, billet, or a shape cast product. Such aluminum casting alloys may realize an improved combination of properties, such as an improved combination of two or more of strength, ductility (elongation), quality index, and bend angle, among others. Additional details are provided below.i. Compositions

[0004] As noted above, the new 3xx aluminum casting alloys generally include from 7.0 to 9.0 wt. % Si, from 0.05 to 0.6 wt. % Mg, from 0.1 to 0.4 wt. % Mn, from 0.05 to 0.25 wt. % Cr, wherein (wt. % Mn) + (wt. % Cr) is from 0.2 to 0.6 wt. %, from 0.05 to 1.5 wt. % Fe, up to 0.5 wt. % Cu, up to 0.5 wt. %Zn, up to 0.15 wt. % Ti, up to 0.15 wt. % V, up to 0.15 wt. % Zr, and up to 0.05 wt. % of any one of Sr, Sb, Na, and Ca, with the balance being aluminum, optional incidental elements, and impurities.

[0005] In one embodiment, a new 3xx aluminum casting alloy includes at least 7.1 wt. % Si. In another embodiment, a new' 3xx aluminum casting alloy includes at least 7.2 wt. % Si. In yet another embodiment, a new 3xx aluminum casting alloy includes at least 7.3 wt. % Si. In another embodiment, a new 3xx aluminum casting alloy includes at least 7.4 wt. % Si. InAttorney Ref. No.: 169593.120026 / WOyet another embodiment, a new 3xx aluminum casting alloy includes at least 7.5 wt. % Si. In another embodiment, a new' 3xx aluminum casting alloy includes at least 7.6 wt. % Si. In yet another embodiment, a new 3xx aluminum casting alloy includes at least 7.7 wt. % Si. In another embodiment, a new 3xx aluminum casting alloy includes at least 7.8 wt. % Si. In yet another embodiment, a new 3xx aluminum casting alloy includes at least 7.9 wt. % Si. In another embodiment, a new 3xx aluminum casting alloy includes at least 8.0 wt. % Si. In yet another embodiment, a new 3xx aluminum casting alloy includes at. least 8.1 wt, % Si. In another embodiment, a new 3xx aluminum casting alloy includes at least 8.2 wt. % Si. In yet another embodiment, a new' 3xx aluminum casting alloy includes at least 8.3 wt. % Si. In another embodiment, a new 3xx aluminum casting alloy includes at least 8.4 wt. % Si.

[0006] In one embodiment, a new 3xx aluminum casting alloy includes not greater than 8.9 wt. % Si. In another embodiment, a new 3xx aluminum casting alloy includes not greater than 8.8 wt. % Si. In yet another embodiment, a new 3xx aluminum casting alloy includes not greater than 8.7 wt. % Si. In another embodiment, a new 3xx aluminum casting alloy includes not greater than 8.6 wt. % Si.

[0007] As noted above, a new 3xx aluminum casting alloy generally includes from 0.05 to 0.6 wt. % Mg. In one embodiment, a new' 3xx aluminum casting alloy includes at least 0.07 wt. % Mg. In another embodiment, a new' 3xx aluminum casting alloy includes at least 0.09 w't. % Mg. In yet another embodiment, a new' 3xx aluminum casting alloy includes at least 0.11 wt. % Mg. In another embodiment, a new' 3xx aluminum casting alloy includes at least 0.13 wt. % Mg, In yet another embodiment, a new 3xx aluminum casting alloy includes at least 0.15 w't. % Mg. In another embodiment, a new' 3xx aluminum casting alloy includes at least 0.17 w't. % Mg. In yet another embodiment, a new' 3xx aluminum casting alloy includes at least 0.19 wt. % Mg. In another embodiment, a new 3xx aluminum casting alloy includes at least 0.20 wt. % Mg.

[0008] In one embodiment, a new' 3xx aluminum casting alloy includes not greater than 0.55 wt. % Mg. In another embodiment, a new 3xx aluminum casting alloy includes not greater than 0,50 wt. % Mg. In yet another embodiment, a new 3xx aluminum casting alloy includes not greater than 0.45 wt. % Mg. In another embodiment, a new' 3xx aluminum casting alloy includes not greater than 0.40 wt. % Mg. In another embodiment, a new' 3xx aluminum casting alloy includes not greater than 0.35 wt. %Mg. In yet another embodiment, a new 3xx aluminum casting alloy includes not greater than 0.30 wt. % Mg. In another embodiment, a new' 3xx aluminum casting alloy includes not greater than 0.25 wt. % Mg. In yet another embodiment,Attorney Ref. No.: 169593.120026 / WOa new 3xx aluminum casting alloy includes not greater than 0.20 wt. % Mg. In another embodiment, anew 3xx aluminum casting alloy includes not greater than 0.15 wt. % Mg.

[0009] As noted above, a new 3xx aluminum casting alloy generally includes from 0,1 to 0.4 wt. % Mn. In one embodiment, a new 3xx aluminum casting alloy includes at least 0.12 wt. % Mn. In another embodiment, a new 3xx aluminum casting alloy includes at least 0.14 wt. % Mn. In yet another embodiment, a new 3xx aluminum casting alloy includes at least 0.16 wt. % Mn, In another embodiment, a new 3xx aluminum casting alloy includes at least 0.18 wt. % Mn.

[0010] In one embodiment, a new' 3xx aluminum casting alloy includes not greater than 0.38 wt. % Mn. In another embodiment, a new 3xx aluminum casting alloy includes not greater than 0.36 wt, % Mn. In yet another embodiment, a new 3xx aluminum casting alloy includes not greater than 0.34 wt. % Mn. In another embodiment, a new 3xx aluminum casting alloy includes not greater than 0.32 wt. % Mn. In yet another embodiment, a new 3xx aluminum casting alloy includes not greater than 0.30 wt. % Mn. In another embodiment, a new 3xx aluminum casting alloy includes not greater than 0.28 wt. % Mn. In yet another embodiment, a new 3xx aluminum casting alloy includes not greater than 0.26 wt. % Mn. In another embodiment, a new 3xx aluminum casting alloy includes not greater than 0.24 wt. % Mn. In yet another embodiment, a new' 3xx aluminum casting alloy includes not greater than 0.22 wt, % Mn.

[0011] As noted above, a new 3xx aluminum casting alloy generally includes from 0.05 to 0.25 wt. % Cr. In one embodiment, a new 3xx aluminum casting alloy includes at least 0.07 wt. % Cr. In another embodiment, a new 3xx aluminum casting alloy includes at least 0.09 wt. % Cr. In yet another embodiment, anew 3xx aluminum casting alloy includes at least 0.11 wt. % Cr. In another embodiment, a new 3xx aluminum casting alloy includes at least 0.13 wt. % Cr.

[0012] In one embodiment, a new 3xx aluminum casting alloy includes not greater than 0.23 wt. % Cr. In another embodiment, a new 3xx aluminum casting alloy includes not greater than 0.21 wt, % Cr. In yet another embodiment, a new 3xx aluminum casting alloy includes not greater than 0.19 wt. % Cr. In another embodiment, a new' 3xx aluminum casting alloy includes not greater than 0.17 wt. % Cr.

[0013] As noted above, a new 3xx aluminum casting alloy generally includes from 0.2. to 0.6 ((wt. % Mn) + (wt, % Cr)), In one embodiment, a new 3xx aluminum casting alloy includes at least 0.22 ((wt. % Mn) + (wt. % Cr)). In another embodiment, a new' 3xx aluminum casting alloy includes at least 0.24 ((wt. % Mn) + (wt. % Cr)). In yet another embodiment, a new 3xxAttorney Ref. No.: 169593.120026 / WOaluminum casting alloy includes at least 0.26 ((wt. % Mn) + (wt. % Cr)). In another embodiment, a new 3xx aluminum casting alloy includes at least 0.28 ((wt. % Mn) + (wt. % Cr)). In yet another embodiment, a new 3xx aluminum casting alloy includes at least 0.30 ((wt. % Mn) + (wt. % Cr)). In another embodiment, a new 3xx aluminum casting alloy includes at least 0.32 ((wt. % Mn) + (wt. % Cr)). In yet another embodiment, a new 3xx aluminum casting alloy includes at least 0.34 ((wt. % Mn) + (wt. % Cr)).

[0014] In one embodiment, a new 3xx aluminum casting alloy includes not greater than 0.55 ((wt. % Mn) + (wt. % Cr)). In another embodiment, a new 3xx aluminum casting alloy includes not greater than 0.50 ((wt. % Mn) + (wt. % Cr)). In yet another embodiment, a new' 3xx aluminum casting alloy includes not greater than 0.45 ((wt. % Mn) + (wt. % Cr)). In another embodiment, a new' 3xx aluminum casting alloy includes not greater than 0.40 ((wt. % Mn) + (wt. % Cr)). In yet another embodiment, a new' 3xx aluminum casting alloy includes not greater than 0.35 ((wt. % Mn) + (wt. % Cr)).

[0015] As noted above, a new' 3xx aluminum casting alloy generally includes from 0.05 to 1.5 wt. % Fe. In one embodiment, a new 3xx aluminum casting alloy includes at least 0.07 wt. % Fe. In another embodiment, a new' 3xx aluminum casting alloy includes at least 0.09 wt. % Fe. In yet another embodiment, a new 3xx aluminum casting alloy includes at least 0.11 wt. % Fe. In another embodiment, a new 3xx aluminum casting alloy includes at least 0.13 wt. % Fe. In yet another embodiment, a new 3xx aluminum casting alloy includes at least 0.15 wt. % Fe. In another embodiment, a new 3xx aluminum casting alloy includes at least 0.17 wt. % Fe. In yet another embodiment, a new 3xx aluminum casting alloy includes at least 0.19 wt. % Fe. In another embodiment, a new 3xx aluminum casting alloy includes at least 0.21 wt. % Fe. In yet another embodiment, a new 3xx aluminum casting alloy includes at least 0.23 wt. % Fe.

[0016] In one embodiment, a new 3xx aluminum casting alloy includes not greater than 1.4 wt, % Fe. In another embodiment, a new? 3xx aluminum casting alloy includes not greater than 1.3 wt. % Fe. In yet another embodiment, a new' 3xx aluminum casting alloy includes not greater than 1.2. wt. % Fe. In another embodiment, a new 3xx aluminum casting alloy includes not greater than 1.1 wt. % Fe, In yet another embodiment, a new 3xx aluminum casting alloy includes not greater than 1.0 wt. % Fe. In another embodiment, a new' 3xx aluminum casting alloy includes not greater than 0.9 w't. % Fe. In yet another embodiment, a new 3xx aluminum casting alloy includes not greater than 0.8 w't. % Fe. In another embodiment, a new' 3xx aluminum casting alloy includes not greater than 0.75 wt. % Fe. In yet another embodiment, a new' 3xx aluminum casting alloy includes not greater than 0.70 wt. % Fe. In another embodiment, a new' 3xx aluminum casting alloy includes not greater than 0.65 wt. % Fe. In yetAttorney Ref. No.: 169593.120026 / WOanother embodiment, a new 3xx aluminum casting alloy includes not greater than 0.60 wt. % Fe. In another embodiment, a new 3xx aluminum casting alloy includes not greater than 0.55 wt. % Fe, In yet another embodiment, a new 3xx aluminum casting alloy includes not greater than 0.50 wt. % Fe. In another embodiment, a new' 3xx aluminum casting alloy includes not greater than 0.45 wt. % Fe. In yet another embodiment, a new' 3xx aluminum casting alloy includes not greater than 0.40 wt. % Fe. In another embodiment, a new' 3xx aluminum casting alloy includes not greater than 0.35 wt. % Fe. In yet another embodiment, a new' 3xx aluminum casting alloy includes not greater than 0.30 wt. % Fe.

[0017] As noted above, a new 3xx aluminum casting alloy generally includes up to 0.5 wt. % Cu. In one embodiment, a new 3xx aluminum casting alloy includes at least 0.02 wt. % Cu. In another embodiment, a new-’ 3xx aluminum casting alloy includes at least 0.04 wt. % Cu. In yet another embodiment, a new 3xx aluminum casting alloy includes at least 0.06 wt. % Cu. In another embodiment, a new 3xx aluminum casting alloy includes at least 0.08 wt. % Cu. In yet another embodiment, a new' 3xx aluminum casting alloy includes at least 0.10 wt. % Cu. In another embodiment, a new' 3xx aluminum casting alloy includes at least 0.12 wt. % Cu. In yet another embodiment, a new 3xx aluminum casting alloy includes at least 0.14 wt. % Cu.

[0018] In one embodiment, a new' 3xx aluminum casting alloy includes not greater than 0.45 wt. % Cu. In another embodiment, a new 3xx aluminum casting alloy includes not greater than 0.40 wt. % Cu. In yet another embodiment, a new 3xx aluminum casting alloy includes not greater than 0.35 wt. % Cu. In another embodiment, a new 3xx aluminum casting alloy includes not greater than 0.30 wt. % Cu. In yet another embodiment, a new 3xx aluminum casting alloy includes not greater than 0.28 w't. % Cu. In another embodiment, a new-’ 3xx aluminum casting alloy includes not greater than 0.26 wt. % Cu. In yet another embodiment, a new 3xx aluminum casting alloy includes not greater than 0.24 wt. % Cu. In another embodiment, a new 3xx aluminum casting alloy includes not greater than 0.22 wt. % Cu. In yet another embodiment, a new 3xx aluminum casting alloy includes not greater than 0.20 wt. % Cu. In another embodiment, a new 3xx aluminum casting alloy includes not greater than 0.18 wt. % Cu, In yet another embodiment, a new 3xx aluminum casting alloy includes not greater than 0.16 wt. % Cu. In another embodiment, a new' 3xx aluminum casting alloy includes not greater than 0.14 wt. % Cu.

[0019] As noted above, a new 3xx aluminum casting alloy generally includes up to 0.5 wt. % Zn. In one embodiment, a new 3xx aluminum casting alloy includes at least 0.02 wt. % Zn. In another embodiment, a new 3xx aluminum casting alloy includes at least 0.04 wt. % Zn. InAttorney Ref. No.: 169593.120026 / WOyet another embodiment, a new 3xx aluminum casting alloy includes at least 0.06 wt. % Zn. In another embodiment, a new 3xx aluminum casting alloy includes at least 0.08 wt. % Zn.

[0020] In one embodiment, a new 3xx aluminum casting alloy includes not greater than 0.45 wt. % Zn. In another embodiment, a new 3xx aluminum casting alloy includes not greater than 0.40 wt. % Zn. In yet another embodiment, a new 3xx aluminum casting alloy includes not greater than 0.35 wt. % Zn. In another embodiment, a new 3xx aluminum casting alloy includes not. greater than 0.30 wt. % Zn. In yet another embodiment, a new 3xx aluminum casting alloy includes not greater than 0.25 wt. % Zn. In another embodiment, a new 3xx aluminum casting alloy includes not greater than 0.23 wt. % Zn. In yet another embodiment, a new 3xx aluminum casting alloy includes not greater than 0.21 wt. % Zn. In another embodiment, anew' 3xx aluminum casting alloy includes not greater than 0.19 wt. %Zn. In yet another embodiment, a new 3xx aluminum casting alloy includes not greater than 0.17 wt. % Zn. In another embodiment, a new 3xx aluminum casting alloy includes not greater than 0.15 wt. % Zn, In yet another embodiment, a new 3xx aluminum casting alloy includes not greater than 0.13 wt. % Zn. In another embodiment, a new 3xx aluminum casting alloy includes not greater than 0.11 wt. % Zn. In yet another embodiment, a new 3xx aluminum casting alloy includes not greater than 0.09 wt. % Zn.

[0021] As noted above, a new 3xx aluminum casting alloy may include up to 0.5 wt. % Cu and up to 0.5 w't. % Zn. In one approach, a new' 3xx aluminum casting alloy includes both copper and zinc. In one embodiment, a new 3xx aluminum casting alloy includes at least 0.02 wt. % Cu and at least 0.02 wt, % Zn. In another embodiment, a new 3xx aluminum casting alloy includes at least 0.08 wt. % Cu and at least 0.08 wt. % Zn. In yet another embodiment, a new 3xx aluminum casting alloy includes at least 0.2 wt. % Cu and 0.2 wt. % Zn. In another embodiment, a new 3xx aluminum casting alloy includes at least 0.2 wt. % Cu and 0.3 wt. % Zn.

[0022] As noted above, a new 3xx aluminum casting alloy generally includes up to 0.15 wt. % Ti. In one embodiment, a new 3xx aluminum casting alloy includes at least 0.005 wt. % Ti. In another embodiment, a new 3xx aluminum casting alloy includes at least 0.01 wt. % Ti. In yet another embodiment, a new 3xx aluminum casting alloy includes at least 0.015 wt. % Ti. In another embodiment, a new 3xx aluminum casting alloy includes at least 0.02 wt. % Ti. In yet another embodiment, a new 3xx aluminum casting alloy includes at least 0.025 wt. % Ti. In another embodiment, a new 3xx aluminum casting alloy includes at least. 0.03 wt. % Ti. In yet another embodiment, a new 3xx aluminum casting alloy includes at least 0.035 wt. % Ti. In another embodiment, a new 3xx aluminum casting alloy includes at least 0.04 wt. % Ti.Attorney Ref. No.: 169593.120026 / WOIn yet another embodiment, a new 3xx aluminum casting alloy includes at least 0.045 w?t. % Ti. In another embodiment, anew 3xx aluminum casting alloy includes at least 0.05 wt. % Ti.

[0023] In one embodiment, a new 3xx aluminum casting alloy includes not greater than 0.14 wt. % Ti. In another embodiment, a new 3xx aluminum casting alloy includes not greater than 0.13 wt. % Ti. In yet another embodiment, a new 3xx aluminum casting alloy includes not greater than 0.12 wt. % Ti. In another embodiment, a new 3xx aluminum casting alloy includes not greater than 0,11 wt. % Ti. In yet another embodiment, a new 3xx aluminum casting alloy includes not greater than 0.10 wt. % Ti. In another embodiment, a new 3xx aluminum casting alloy includes not greater than 0.09 wt. % Ti. In yet another embodiment, a new 3xx aluminum casting alloy includes not greater than 0.08 wt. % Ti.

[0024] As noted above, a new 3xx aluminum casting alloy generally includes up to 0.15 wt. % V. In one embodiment, a new' 3xx aluminum casting alloy includes at least 0.005 wt. % V. In another embodiment, a new 3xx aluminum casting alloy includes at least 0.01 wt. % V. In yet another embodiment, a new? 3xx aluminum casting alloy includes at least 0.015 wt. % V. In another embodiment, a new? 3xx aluminum casting alloy includes at least 0.02 wt. % V. In yet another embodiment, a new' 3xx aluminum casting alloy includes at least 0.025 wt. % V. In another embodiment, a new 3xx aluminum casting alloy includes at least 0.03 wt. % V. In yet another embodiment, a new' 3xx aluminum casting alloy includes at least 0.035 wt, % V. In another embodiment, a new? 3xx aluminum casting ahoy includes at least 0.04 wt. % V. In yet another embodiment, a new 3xx aluminum casting alloy includes at least 0.045 wt. % V. In another embodiment, anew? 3xx aluminum casting alloy includes at least 0.05 wt, % V.

[0025] In one embodiment, a new? 3xx aluminum casting alloy includes not greater than 0.14 wt. % V. In another embodiment, a new 3xx aluminum casting alloy includes not greater than 0.13 wt. % V. In yet another embodiment, a new 3xx aluminum casting alloy includes not greater than 0.12 wt. % V. In another embodiment, a new? 3xx aluminum casting alloy includes not greater than 0.11 w't. % V. In yet another embodiment, a new' 3xx aluminum casting alloy includes not greater than 0.10 wt. % V. In another embodiment, a new? 3xx aluminum casting alloy includes not greater than 0.09 wt. % V, In yet another embodiment, a new? 3xx aluminum casting alloy includes not greater than 0.08 w?t. % V.

[0026] As noted above, a new' 3xx aluminum casting alloy generally includes up to 0.15 wt. % Zr. In one embodiment, a new 3xx aluminum casting alloy includes at least 0.005 wt. % Zr. In another embodiment, a new? 3xx aluminum casting alloy includes at least 0.01 wt. % Zr. In yet another embodiment, a new? 3xx aluminum casting alloy includes at least 0.015 wt. % Zr. In another embodiment, a new 3xx aluminum casting alloy includes at least 0.02 wt. % Zr.Attorney Ref. No.: 169593.120026 / WOIn yet another embodiment, a new 3xx aluminum casting alloy includes at least 0.025 wt. % Zr. In another embodiment, a new 3xx aluminum casting alloy includes at least 0.03 wt. % Zr. In yet another embodiment, a new 3xx aluminum casting alloy includes at least 0.035 wt. % Zr. In another embodiment, a new 3xx aluminum casting alloy includes at least 0.04 wt. % Zr. In yet another embodiment, a new 3xx aluminum casting alloy includes at least 0.045 wt. % Zr. In another embodiment, a new 3xx aluminum casting alloy includes at least 0.05 wt. % Zr.[002.7] In one embodiment, a new 3xx aluminum casting alloy includes not greater than 0.14 wt. % Zr. In another embodiment, a new 3xx aluminum casting alloy includes not greater than 0.13 wt. % Zr. In yet another embodiment, a new 3xx aluminum casting alloy includes not greater than 0.12 wt. % Zr. In another embodiment, a new 3xx aluminum casting alloy includes not greater than 0.11 wt. % Zr. In yet another embodiment, a new' 3xx aluminum casting alloy includes not greater than 0.10 wt. % Zr. In another embodiment, a new 3xx aluminum casting alloy includes not greater than 0.09 wt. % Zr. In yet another embodiment, a new' 3xx aluminum casting alloy includes not greater than 0.08 wt. % Zr.

[0028] In one embodiment, a new 3xx aluminum casting alloy includes both at least 0.03 wt. % V and at least 0.03 wt. % Zr. In another embodiment, a new' 3xx aluminum casting alloy includes both at least 0.05 wt. % V and at least 0.10 wt. % Zr.

[0029] As noted above, a new' 3xx aluminum casting alloy generally includes up to 0.05 wt. % Sr. In one embodiment, anew 3xx aluminum casting alloy includes at least 50 ppm Sr. In another embodiment, anew' 3xx aluminum casting alloy includes at least 100 ppm Sr. In yet another embodiment, a new 3xx aluminum casting alloy includes at least 150 ppm Sr. In another embodiment, a new? 3xx aluminum casting alloy includes at least 200 ppm Sr. In yet another embodiment, a new' 3xx aluminum casting alloy includes at least 250 ppm Sr. In another embodiment, a new 3xx aluminum casting alloy includes at least 300 ppm Sr.

[0030] As noted above, a new' 3xx aluminum casting alloy generally includes up to 0.05 't. % Sb. In one embodiment, a new' 3xx aluminum casting alloy includes at least 50 ppm Sb. In another embodiment, a new 3xx aluminum casting alloy includes at least 100 ppm Sb. In yet another embodiment, a new 3xx aluminum casting alloy includes at least 150 ppm Sb. In another embodiment, a new' 3xx aluminum casting alloy includes at least 200 ppm Sb. In yet another embodiment, a new' 3xx aluminum casting alloy includes at least 250 ppm Sb. In another embodiment, a new 3xx aluminum casting alloy includes at least 300 ppm Sb.

[0031] As noted above, a new' 3xx aluminum casting alloy generally includes up to 0.05 w't. % Na. In one embodiment, a new' 3xx aluminum casting alloy includes at least 50 ppm Na. In another embodiment, a new 3xx aluminum casting alloy includes at least 100 ppm Na. InAttorney Ref. No.: 169593.120026 / WOyet another embodiment, a new 3xx aluminum casting alloy includes at least 150 ppm Na. In another embodiment, a new' 3xx aluminum casting alloy includes at least 200 ppm Na. In yet another embodiment, a new 3xx aluminum casting alloy includes at least 250 ppm Na. In another embodiment, a new 3xx aluminum casting alloy includes at least 300 ppm Na.

[0032] As noted above, a new 3xx aluminum casting alloy generally includes up to 0.05 wt. % Ca. In one embodiment, a new 3xx aluminum casting alloy includes at least 50 ppm Ca. In another embodiment, a new 3xx aluminum casting alloy includes at least 100 ppm Ca. In yet another embodiment, a new' 3xx aluminum casting alloy includes at least 150 ppm Ca. In another embodiment, a new' 3xx aluminum casting alloy includes at least 200 ppm Ca. In yet another embodiment, a new' 3xx aluminum casting alloy includes at least 250 ppm Ca. In another embodiment, a new' 3xx aluminum casting alloy includes at least 300 ppm Ca.

[0033] In one embodiment, a new' 3xx aluminum casting alloy includes about 7.0-8.5 wt. % Si, 0.05-0.20 wt. % Mg, 0.05-0.20 wt. % Cu, 0.07-0.20 wt. % Cr, optionally 0.05-0.18 wt. % Zr, 0.10-0.35 wt. % Fe, from 50 to 500 ppm of Sr, and up to 0.50 wt. % Zn, the balance being aluminum, optional incidental elements, and impurities.

[0034] As noted above, the balance of the new' 3xx aluminum alloy products is generally aluminum, optional incidental elements, and impurities. As used herein, ‘’incidental elements” means those elements or materials, other than the above listed elements, that may optionally be added to the alloy to assist in the production of the alloy. Examples of incidental elements include casting aids, such as grain refiners and deoxidizers. Optional incidental elements may be included in the alloy in a cumulative amount of up to 1.0 wt. %. Examples of some deoxidizers include Ca, Sr, and Be. When calcium (Ca) is included in the alloy, it is generally present in the amounts described previously herein. Strontium (Sr) may be included in the alloy as a substitute for Ca (m whole or m part), and thus may be included in the alloy in the same or similar amounts as Ca. Traditionally, beryllium (Be) additions have helped to reduce the tendency of ingot cracking, though for environmental, health, and safety' reasons, some embodiments of the alloy are substantially Be-free. When Be is included in the alloy, it is generally present in an amount of up to about 20 ppm. Incidental elements may be present in minor amounts, or may be present in significant amounts, and may add desirable or other characteristics on their own without departing from the alloy described herein, so long as the alloy retains the desirable characteristics described herein. It is to be understood, however, that the scope of this disclosure should not / cannot be avoided through the mere addition of an element or elements in quantities that would not otherwise impact on the combinations of properties desired and attained herein.Attorney Ref. No.: 169593.120026 / WO

[0035] The new 3xx aluminum casting alloys may contain low amounts of impurities. In one embodiment, a 3xx aluminum casting alloy includes not greater than 0.15 wt. %, in total, of the impurities, and wherein the 3 x aluminum casting alloy includes not greater than 0.05 wt. % of each of the impurities. In another embodiment, the 3xx aluminum casting alloy includes not greater than 0.10 wt. %, in total, of the impurities, and wherein the 3xx aluminum casting alloy includes not greater than 0.03 wt. % of each of the impurities.

[0036] The new 3xx aluminum casting alloys are generally substantially free of molybdenum, i.e., molybdenum is included only as an impurity, and generally at less than 0.04 wt. % Mo, or less than 0.01 wt. % Mo. The new 3xx aluminum casting alloys are generally substantially free of lithium, i.e., lithium is included only as an impurity, and generally at less than 0.04 wt. % Li, or less than 0.01 wt. % Li. The new 3xx aluminum casting alloys are generally substantially free of silver, i.e., silver is included only as an impurity, and generally at less than 0.04 wt. % Ag, or less than 0.01 wt. % Ag. The new 3xx aluminum casting alloys are generally substantially free of lead, i.e., lead is included only as an impurity, and generally at less than 0.04 wt. % Pb, or less than 0.01 wt. % Pb. Tire new 3xx aluminum casting alloys are generally substantially free of cadmium, i.e., cadmium is included only as an impurity, and generally at less than 0.04 wt. % Cd, or less than 0.01 wt. % Cd. The new 3xx aluminum casting alloys are generally substantially free of tin, i.e., tin is included only as an impurity, and generally at less than 0.04 wt. % Sn, or less than 0.01 wt. % Sn. The new 3xx aluminum casting alloys are generally substantially free of bismuth, i.e., bismuth is included only as an impurity, and generally at less than 0.04 wt. % Bi, or less than 0.01 wt. % Bi,zz. Methods of Manufacture

[0037] As noted above, a new 3xx aluminum casting alloy may be produced by an aluminum casting process. In one embodiment, as illustrated in FIG. 2, a casting process may include: filling a shape casting mold with a molten aluminum alloy (100), wherein the molten aluminum alloy has a composition as per Section i, Compositions, cooling the molten aluminum alloy within the shape casting mold (200), and extracting the final shape cast product from the shape casting mold (300).

[0038] Use of Recycle Material

[0039] In one embodiment, and with reference to FIG. 2, the filling step (100) comprises melting (110) an aluminum alloy ingot or billet having a composition as per Section i, Compositions, and adding that molten aluminum alloy to the shape casting mold. In one embodiment, an ingot or billet is produced by using (120) at least 50 % recycled aluminum. For instance, to produce the desired chemistry / composition, an ingot or billet is produced byAttorney Ref. No.: 169593.120026 / WOmixing at least 50 % recycled aluminum with primary aluminum, and / or one or more master alloys and / or other materials sufficient to achieve a target chemistry, wherein the target chemistry is any of the compositions described in Section i, Compositions. In one embodiment, an ingot or billet is produced by mixing at least 55 % recycled aluminum with primary aluminum, and / or one or more master alloys and / or other materials sufficient to achieve a target chemistry, wherein the target chemistry is any of the compositions described in Section i, Compositions. In another embodiment, an ingot or billet is produced by mixing at least 60 % recycled aluminum with primary aluminum, and / or one or more master alloys and / or other materials sufficient to achieve a target chemistry, wherein the target chemistry is any of the compositions described in Section i, Compositions. In yet another embodiment, an ingot or billet is produced by mixing at least 65 % recycled aluminum with primary aluminum, and / or one or more master alloys and / or other materials sufficient to achieve a target chemistry, wherein the target chemistry is any of the compositions described in Section i, Compositions. In another embodiment, an ingot or billet is produced by mixing at least 75 % recycled aluminum with primary aluminum, and / or one or more master alloys and / or other materials sufficient to achieve a target chemistry, wherein the target chemistry is any of the compositions described in Section i, Compositions. In yet another embodiment, an ingot or billet is produced by mixing at least 80 % recycled aluminum with primary aluminum, and / or one or more master alloys and / or other materials sufficient to achieve a target chemistry, wherein the target chemistry is any of the compositions described in Section i, Compositions. In another embodiment, an ingot or billet is produced by mixing at least 85 % recycled aluminum with primary' aluminum, and / or one or more master alloys and / or other materials sufficient to achieve a target chemistry, wherein the target chemistry is any of the compositions described in Section i, Compositions. In yet another embodiment, an ingot or billet is produced by mixing at least 90 % recycled aluminum with primary aluminum, and / or one or more master alloys and / or other materials sufficient to achieve a target chemistry, wherein the target chemistry is any of the compositions described in Section i, Compositions. In another embodiment, an ingot or billet is produced by mixing at least 95 % recycled aluminum with primary aluminum, and / or one or more master alloys and / or other materials sufficient to achieve a target chemistry, wherein the target chemistry is any of the compositions described in Section i, Compositions.

[0040] As used herein, ‘"recycled aluminum'’ means aluminum obtained from any suitable scrap aluminum source, as opposed to primary aluminum obtained from an aluminum electrolysis cell. Any suitable scrap aluminum may be used as a source of the recycled aluminum, and may include scrap aluminum from various sources, such as scrap of a Ixxx,Attorney Ref. No.: 169593.120026 / WO2xxx, 3xxx, 4xxx, 5xxx, 6xxx, 7xxx, or 8xxx aluminum alloy composition or their casting alloy equivalent. In one embodiment, the scrap at least partially includes toothpaste tube scrap. Other suitable scrap sources include automotive scrap (e.g., from prior used vehicles, including from door panels, bumpers, engines, and structural members, among others), brazing scrap (e.g., from tube stock, headers, or other heat exchanger materials, among others), used beverage cans (LBC) scrap, aerospace scrap, and industrial scrap, among others.

[0041] Shape Casting

[0042] As noted above, a new 3xx aluminum casting alloy may be produced by filling a shape casting mold with a molten aluminum alloy (100). In one embodiment, the molten aluminum alloy may be at a temperature of at least 3° C above the liquidus temperature of the aluminum alloy. In another embodiment, the molten aluminum alloy may be at a temperature of at least 5° C above the liquidus temperature of the aluminum alloy. In yet another embodiment, the molten aluminum alloy may be at a temperature of at least 8° C above the liquidus temperature of the aluminum alloy. In another embodiment, the molten aluminum alloy may be at a temperature of at least 10° C above the liquidus temperature of the aluminum alloy. In yet another embodiment, the molten aluminum alloy may be at a temperature of at least 15° C above the liquidus temperature of the aluminum alloy. In another embodiment, the molten aluminum alloy may be at a temperature of at least 20° C above the liquidus temperature of the aluminum alloy. In yet another embodiment, the molten aluminum alloy may be at a temperature of at least 30° C above the liquidus temperature of the aluminum alloy. In another embodiment, the molten aluminum alloy may be at a temperature of at least 40° C above the liquidus temperature of the aluminum alloy. In yet another embodiment, the molten aluminum alloy may be at a temperature of at least 50° C above the liquidus temperature of the aluminum alloy. In another embodiment, the molten aluminum alloy may be at a temperature of at least 60° C above the liquidus temperature of the aluminum alloy. In yet another embodiment, the molten aluminum alloy may be at a temperature of at least 70° C above the liquidus temperature of the aluminum alloy. In another embodiment, the molten aluminum alloy may be at a temperature of at least 80° C above the liquidus temperature of the aluminum alloy. In yet another embodiment, the molten aluminum alloy may be at a temperature of at least 90° C above the liquidus temperature of the aluminum alloy. In another embodiment, the molten aluminum alloy may be at a temperature of at least 100° C above the liquidus temperature of the aluminum alloy.

[0043] In one embodiment, and with reference to FIG. 25, after filling the shape casting mold with a molten aluminum alloy (100), a molten aluminum alloy may be cooled within theAttorney Ref. No.: 169593.120026 / WOshape casting mold (200). In one embodiment, cooling the molten aluminum alloy within the shape casting mold (200) may include solidifying the molten aluminum alloy (210), thereby creating a shape cast product. In one embodiment, cooling the shape cast product may comprise applying a coolant to the shape casting mold (220). In one embodiment, the mold may be a die¬ casting mold, an investment casting mold, a low pressure or gravity casting mold, permanent or semi-permanent mold, a squeeze casting mold, a high pressure die casting mold, a low- pressure sand-casting (LPSC) mold, a directional casting mold, or sand mold casting. In one embodiment, the shape casting mold is a megacasting mold (i.e., a mold suited for producing a megacasting). In one embodiment, the molten metal aluminum alloy is a thixotropic metal mass and forming the aluminum alloy product comprises semi-solid casting or forming.

[0044] In one embodiment, cooling the molten aluminum alloy within the shape casting mold (200) may include applying pressure to the molten aluminum alloy (230). In one embodiment, the applying pressure to the molten aluminum alloy (230) step may be performed using high pressure or low pressure. In one embodiment, the applied pressure is at least 10 MPa, which relates to high-pressure die casting. In another embodiment, the applied pressure is at least 20 MPa. In yet another embodiment, the applied pressure is at least 30 MPa. In another embodiment, the applied pressure is at least 40 MPa. In yet another embodiment, the applied pressure is at least 50 MPa, In another embodiment, the applied pressure is at least 75 MPa. In yet another embodiment, the applied pressure is at least 100 MPa. In another embodiment, the applied pressure is at least 125 MPa. In yet another embodiment, the applied pressure is at least 150 MPa. In another embodiment, the applied pressure is at least 175 MPa. In one embodiment, due to the applied pressure, the shape cast product may be a high-pressure die-cast (HPDC) shape cast product.

[0045] In one embodiment, the filling the shape casting mold (100) step and the cooling the molten aluminum alloy within the shape casting mold (200) step may be performed using a machine, such as a HPDC machine, or a. vacuum assisted HPDC machine, among others. In one embodiment, the machine is graded to supply a force of at least 250 tons. In another embodiment, the machine is graded to supply a force of at least 500 tons. In yet another embodiment, the machine is graded to supply a force of at least 750 tons. In another embodiment, the machine is graded to supply a force of at least 1,000 tons. In yet another embodiment, the machine is graded to supply a force of at least 2,000 tons. In another embodiment, the machine is graded to supply a force of at least 3,000 tons. In yet another embodiment, the machine is graded to supply a force of at least 4,000 tons. In another embodiment, the machine is graded to supply a force of at least 5,000 tons. In yet anotherAttorney Ref. No.: 169593.120026 / WOembodiment, the machine is graded to supply a force of at least 6,000 tons. In another embodiment, the machine is graded to supply a force of at least 7,000 tons. In yet another embodiment, the machine is graded to supply a force of at least 8,000 tons. In another embodiment, the machine is graded to supply a force of at least 9,000 tons. In yet another embodiment, the machine is graded to supply a force of at least 10,000 tons. In another embodiment, the machine is graded to supply a force of at least 11,000 tons. In yet another embodiment, the machine is graded to supply a force of at least 12,000 tons. In another embodiment, the machine is graded to supply a force of at least 13,000 tons. In yet another embodiment, the machine is graded to supply a force of at least 14,000 tons. In another embodiment, the machine is graded to supply a force of at least 15,000 tons. In yet another embodiment, the machine is graded to supply a force of at least 16,000 tons. In another embodiment, the machine is graded to supply a force of at least 17,000 tons. In yet another embodiment, the machine is graded to supply a force of at least 18,000 tons. In another embodiment, the machine is graded to supply a force of at least 19,000 tons. In yet another embodiment, the machine is graded to supply a force of at least 20,000 tons.

[0046] As noted above, after the cooling of the molten aluminum alloy within the shape casting mold (200) step, the shape cast product may be extracted from the shape casting mold (300). In one embodiment, and with reference to FIG. 26, after the shape cast product, is removed from the shape casting mold (300), the shape cast product may be non-porous (310), i.e., has little or no porosity as observed under visual inspection and / or microscopic inspection and / or is suited for its intended use due to it being non-porous, understanding some minimal porosity may be present that does not materially affect the properties of the shape cast product. In one embodiment, after the shape cast product is removed from the shape casting mold (300), the shape cast product may be substantially surface defect-free (320), i.e., has very few or no observable surface detects and / or is suited for its intended use due to it being substantially surface defect-free, understanding some minimal defects may be present that does not materially affect the properties of the shape cast product. In one embodiment, and with reference to FIG. 26, afterthe shape cast product, is removed from the shape casting mold (300), the shape cast product is a megacasting (330). In one embodiment, a. megacasting is substantially free of other defects, such as one or more of trapped air, oxides, cold shuts, and misruns, among others.

[0047] The shape cast product may be used in any suitable application, such as in an automotive, aerospace or industrial application. In one embodiment, the shape cast product is an automotive product, such as for a gasoline powered vehicle, a battery powered electricAttorney Ref. No.: 169593.120026 / WOvehicle (BEV), or hybrid (gas+electric) powered vehicle. The shape cast automotive product may be, for instance, a chassis (e.g., for the front and / or rear underbody sections of an automotive vehicle), a shock tower, a cross member, a B-piilar, a frame rail, a cargo floor reinforcement, a tank cover frame, a reinforcement side member, a battery tray, an electric drive unit component, a transmission housing, a rear floor frame, a front cabin, a batery box, a full frame, an engine cylinder head, and / or an engine block, among others. In one embodiment, the shape cast automotive product may be a shape cast automotive product for a battery electric vehicle (BEV), for instance, a battery tray and / or an electric drive unit component, among others.

[0048] In one embodiment, the shape cast product may be a megacasting. A megacasting is a monolithic (single cast piece) shape cast product having at least one dimension that is at least 0.25 meters in length, width, and / or height. For instance, a shape cast product (e.g., an automotive shape cast product for use in a vehicle), may have at least one feature that is at least 0.25 meters in length, width, and / or height. In one embodiment, a megacasting has at least one feature that is at least 0.50 meters in length, width, and / or height. In another embodiment, a megacasting has at least one feature that is at least 0.75 meters in length, width, and / or height. In yet another embodiment, a megacasting has at least one feature that is at least 1.0 meters in length, width, and / or height. In another embodiment, a megacasting has at least one feature that is at least 1.25 meters in length, width, and / or height. In yet another embodiment, a megacasting has at least one feature that is at least 1.50 meters in length, width, and / or height. In another embodiment, a megacasting has at least one feature that is at least 1.75 meters in length, width, and / or height. In yet another embodiment, a megacasting has at least one feature that is at least 2.0 meters in length, width, and / or height. In another embodiment, a megacasting has at least one feature that is at least 2.5 meters in length, width, and / or height. In yet another embodiment, a megacasting has at least one feature that is at least 3.0 meters in length, width, and / or height. In another embodiment, a megacasting has at least one feature that is at least 3.5 meters in length, width, and / or height. In yet another embodiment, a megacasting has at least one feature that is at least 4.0 meters in length, width, and / or height. In another embodiment, a megacasting has at least one feature that is at least 4.5 meters in length, width, and / or height. In yet another embodiment, a megacasting has at least one feature that is at least 5.0 meters in length, width, and / or height. As used herein, “megacastings” includes other terms known in the art, such as “gigacastings.”

[0049] In one embodiment, and with reference to FIG. 26, after the shape cast product is extracted from the shape casting mold (300), the shape cast product may be a megacastingAttorney Ref. No.: 169593.120026 / WO(330). In one embodiment, a megacasting is a single-piece panel that serves as a load bearing structure of a vehicle body. In another embodiment, a megacasting is a structural component that serves as a load bearing structure of the vehicle body. A single megacasting may be used in place of multiple structures. For example, a single megacasting may be used in place of multiple parts that are joined together. One embodiment of a megacasting is illustrated in FIG.22, which illustrates a vehicle (1000) including a vehicle body structure (1001) including a megacasting (2000) acting as an energy absorbing system. The megacasting (2000) may be made from any of the new 3xx aluminum casting alloy compositions described in Section I, Compositions. The megacasting (2000) may be manufactured with very large parts from a single casting, in other words by a megacasting process. Such megacastings (2000) can be positioned at a front floor portion (2100) and / or a rear floor portion (2200) of the vehicle body structure (1001). In one embodiment, a megacasting (2000) is used as an element of a cabin portion (1100) of the vehicle body structure (1001). In one embodiment, a megacasting (2000) is used as an element of a front part ( 1200) of the vehicle body structure. In one embodiment, a megacasting (2000) is used as an element of a rear part (1300) of the vehicle body structure (1001). In one embodiment, the megacasting (2000) is be used as an element of an A-pillar portion (1400) of the vehicle body structure (1001).

[0050] The mold used to produce the shape cast product, including any megacastings, may have a size that varies in one or more dimensions to achieve, for instance, the intricate features of the shape cast product. For instance, the mold may include one or more arcuate surfaces, which arcuate surface(s) may correspond to arcuate surface of the final shape cast product. The mold may also include one or more indentations, which indentation(s) may correspond to protrusions of the final shape cast product. The mold may also include one or more extensions, which extension(s) may correspond to indentation(s) and / or aperture(s) of the final shape cast product. In one embodiment, the aperture(s) are suited for use in attaching the shape cast product to one or more other structures, such as one or more structure(s) used in an automobile structure, an aerospace structure, or an industrial application structure. In one embodiment, and with reference to FIG, 26, after the final shape cast product is extracted from the shape casting mold (300), the shape cast product may have a plurality of predetermined arcuate features and / or a plurality of predetermined apertures (340).

[0051] Tire shape cast product may have any suitable thickness. In one embodiment, the thickness of the shape cast product is at least 1 mm. In another embodiment, the thickness of the shape cast product is at least 3 mm. In yet another embodiment, the thickness of the shape cast product is at least 5 mm. In another embodiment, the thickness of the shape cast productAttorney Ref. No.: 169593.120026 / WOis at least 10 mm. In one embodiment, a shape cast product may have a uniform thickness (e.g., + / - 20 % across the applicable dimensions of the shape cast product). In one embodiment, a megacasting includes varying wall thicknesses at least partially throughout, or completely throughout the megacasting. In one embodiment, a megacasting comprises ribs and / or bosses, whose thickness is at least two times that of the nominal thickness of the adjacent walls of the megacasting. In one embodiment, the ribs and / or bosses are substantially non-porous.

[0052] Post-Casting Processing

[0053] As noted above, after casting, the shape cast product may be extracted from the shape casting mold (300). In one embodiment, and with reference to FIG. 27, after the shape cast product is extracted from the shape casting mold (300), the shape cast product may be aged (400). In one embodiment, the aging includes natural aging. Natural aging may include aging the shape cast product at substantially ambient conditions (e.g., ambient temperature) for a period of at least 24 hours. In one embodiment, the natural aging time is at least 2 days. In another embodiment, the natural aging time is at least 3 days. In yet another embodiment, the natural aging time is at least 4 days. In another embodiment, the natural aging time is at least 5 days. In another embodiment, the natural aging time is at least 7 days. In yet another embodiment, the natural aging time is at least 10 days. In another embodiment, the natural aging time is at least 15 days. In yet another embodiment, the natural aging time is at least 20 days. In another embodiment, the natural aging time is at least 25 days. In yet another embodiment, the natural aging time is at least 30 days. In another embodiment, the natural aging time is at least 35 days. In yet another embodiment, the natural aging time is at least 40 days. In another embodiment, the natural aging time is at least 45 days.

[0054] During or after natural aging, the shape cast product may be shipped (500) to a customer and / or artificially aged. In one embodiment, a shape cast product is shipped in an F- temper or in a naturally aged temper. In one embodiment, any artificial aging is performed by the customer (e.g., as part of a paint-bake process). In one embodiment, the artificial aging comprises applying (601) one or more coatings to the shape cast product and then paint baking (applying heat) for a time sufficient to properly cure the paint or other coatings located on the shape cast product while also achieving at least some precipitation hardening of the shape cast aluminum alloy product. For instance, the artificial aging may include exposing the shape cast product to a temperature of at least 195° C for at least 45 minutes. In one embodiment, the one or more coatings may increase the corrosion resistance of the shape cast product. Before and / or after a coating is applied to the shape cast product (601), a final shape cast product may beAttorney Ref. No.: 169593.120026 / WOattached to a vehicle (602). The final shape cast product may be one component of a plurality of components of the vehicle.

[0055] As noted above, the shape cast product may be produced or realize a naturally aged or an artificially aged temper. Separate or integrated solution heat treatment may be used as needed to dissolve soluble precipitate phases. Thus, the shape cast product may be in or realize any one of a Tl, T2, T3, T4, T5, T6, T7, T8, T9, or T10 temper. The shape cast product may also be in or realize an F-temper (as fabricated), an O-temper (annealed), or a W-temper (solution heat treated).

[0056] As noted above, the shape cast product may attached to one or more structures. In one embodiment, the shape cast product may be attached to the one or more structures using rivets. Indeed, as noted herein, due to the unique composition and / or microstructure of the shape cast aluminum alloy products described herein, a shape cast product may be successfully rivetted to steel and / or other materials, making it uniquely suited for many applications in which joining is required. In one embodiment, the rivets include self-piercing rivets. In one embodiment, the shape cast product may be attached to one or more structures via welding. In one embodiment, the shape cast product may be aged after the shape cast product is attached to one or more structures.Microstructure

[0057] As noted above, the new 3xx aluminum casting alloys may realize an improved combination of properties, such as an improved combination of two or more of ultimate tensile strength, tensile yield strength, ductility (elongation), quality index, and bend angle, among others. The improved properties may be at least partially due to the microstructure of the alloy.

[0058] In one approach, a new 3xx aluminum casting alloy (e.g., a shape cast product) includes at least some FeCrMn intermetallic particles. In one embodiment, at least some of the FeCrMn intermetallic particles are spheroidal FeCrMn intermetallic particles. In one embodiment, the spheroidal FeCrMn intermetallic particles realize an aspect ratio of not greater than 5:1. In another embodiment, the spheroidal FeCrMn intermetallic particles realize an aspect ratio of not greater than 4:1. In yet another embodiment, the spheroidal FeCrMn intermetallic particles realize an aspect ratio of not greater than 3:1. In another embodiment, the spheroidal FeCrMn intermetallic particles realize an aspect, ratio of not greater than 2: 1. In yet another embodiment, the spheroidal FeCrMn intermetallic particles realize an aspect ratio of not greater than 1.5:1.

[0059] In one embodiment, a new 3xx aluminum casting alloy includes a volume fraction of FeMnCr intermetallic particles, and at least 40 vol. % of the FeMnCr intermetallic particlesAttorney Ref. No.: 169593.120026 / WOare spheroidal FeCrMn intermetallic particles. In another embodiment, at least 50 vol. % of the FeMnCr intermetallic particles are spheroidal FeCrMn intermetallic particles. In yet another embodiment, at least 60 vol. % of the FeMnCr intermetallic particles are spheroidal FeCrMn intermetallic particles. In another embodiment, at least 70 vol. % of the FeMnCr intermetallic particles are spheroidal FeCrMn intermetallic particles. In yet another embodiment, at least 80 vol. % of the FeMnCr intermetallic particles are spheroidal FeCrMn intermetallic particles. In another embodiment, at least 90 vol. % of the FeMnCr intermetallic particles are spheroidal FeCrMn intermetallic particles. In yet another embodiment, at least 95 vol. % of the FeMnCr intermetallic particles are spheroidal FeCrMn intermetallic particles. In another embodiment, at least 98 vol. % of the FeMnCr intermetallic particles are spheroidal FeCrMn intermetallic particles. In yet another embodiment, at least 99 vol. % of the FeMnCr intermetallic particles are spheroidal FeCrMn intermetallic particles.iii. Properties

[0060] As noted above, shape cast products made from the new 3xx aluminum casting alloys may realize an improved combination of properties, such as an improved combination of two or more of ultimate tensile strength, tensile yield strength, ductility (elongation), quality index, and bend angle, among others.

[0061] In one embodiment, a new 3xx shape cast product realizes an ultimate tensile strength (UTS) of at least 250 MPa. In another embodiment, a new 3xx shape cast product realizes an ultimate tensile strength of at least 255 MPa. In yet another embodiment, a new 3xx shape cast product realizes an ultimate tensile strength of at least 260 MPa. In another embodiment, a new 3xx shape cast product realizes an ultimate tensile strength of at least 265 MPa. In yet another embodiment, a new 3xx shape cast product realizes an ultimate tensile strength of at least 270 MPa. In another embodiment, a new 3xx shape cast product realizes an ultimate tensile strength of at least 275 MPa. In yet another embodiment, a new 3xx shape cast product realizes an ultimate tensile strength of at least 280 MPa. In another embodiment, a new 3xx shape cast product realizes an ultimate tensile strength of at least 285 MPa. In yet another embodiment, a new 3xx shape cast product realizes an ultimate tensile strength of at least 290 MPa. In another embodiment, a new 3xx shape cast product realizes an ultimate tensile strength of at least 295 MPa. In yet another embodiment, a new 3xx shape cast product realizes an ultimate tensile strength of at least 300 MPa.

[0062] In one embodiment, a new 3xx shape cast product realizes a tensile yield strength of at least 100 MPa. In another embodiment, a new 3xx shape cast product realizes a tensile yield strength of at least 105 MPa. In yet another embodiment, a new' 3xx shape cast productAttorney Ref. No.: 169593.120026 / WOrealizes a tensile yield strength of at least 110 MPa. In another embodiment, a new 3xx shape cast product realizes a tensile yield strength of at least 115 MPa. In yet another embodiment, a new 3xx shape cast product realizes a tensile yield strength of at least 120 MPa, In another embodiment, a new 3xx shape cast product realizes a tensile yield strength of at least 125 MPa. In yet another embodiment, a new 3xx shape cast product realizes a tensile yield strength of at least 130 MPa. In another embodiment, a new 3xx shape cast product realizes a tensile yield strength of at least 135 MPa. In yet another embodiment, a new 3xx shape cast product realizes a tensile yield strength of at least 140 MPa.

[0063] In one embodiment, a new 3xx shape cast product realizes an elongation of at least 5 %. In another embodiment, a new 3xx shape cast product realizes an elongation of at least 6 %. In yet another embodiment, a new 3xx shape cast product realizes an elongation of at least 7 %. In another embodiment, a new 3xx shape cast product realizes an elongation of at least 8 %. In yet another embodiment, a new 3xx shape cast product realizes an elongation of at least 9 %. In another embodiment, a new 3xx shape cast product realizes an elongation of at least 10 %. In yet another embodiment, a new 3xx shape cast product realizes an elongation of at least 11 %. In another embodiment, a new 3xx shape cast product realizes an elongation of at least 12 %. In yet another embodiment, a new 3xx shape cast product realizes an elongation of at least 13 %. In another embodiment, a new 3xx shape cast product realizes an elongation of at least 14 %. In yet another embodiment, a new 3xx shape cast product realizes an elongation of at least 15 %.

[0064] In one embodiment, a new 3xx shape cast product realizes a quality index of at least 425. In another embodiment, a new 3xx shape cast product realizes a quality index of at least 430. In yet another embodiment, a new 3xx shape cast product realizes a quality index of at least 435. In another embodiment, a new 3xx shape cast product realizes a quality index of at least 440. In yet another embodiment, a new 3xx shape cast product realizes a quality index of at least 445. In another embodiment, a new 3xx shape cast product realizes a quality index of at least 450. In yet another embodiment, a new 3xx shape cast product realizes a quality index of at least 455.

[0065] In one embodiment, a new 3xx shape cast product realizes a bend angle of at least 31.5°. In another embodiment, a new 3xx shape cast product realizes a bend angle of at least 32°. In yet another embodiment, a new 3xx shape cast product realizes a bend angle of at least 32.5°. In another embodiment, a new 3xx shape cast product realizes a bend angle of at least 33°. In yet another embodiment, a new 3xx shape cast product realizes a bend angle of at least 33.5°. In another embodiment, a new 3xx shape cast product realizes a bend angle of at leastAttorney Ref. No.: 169593.120026 / WO34°. In yet another embodiment, a new 3xx shape cast product realizes a bend angle of at least 34.5°. In another embodiment, a new 3xx shape cast product realizes a bend angle of at least 35°. In yet another embodiment, a new 3xx shape cast product realizes a bend angle of at least 35.5°. In another embodiment, a new 3xx shape cast product realizes a bend angle of at least 36°. In yet another embodiment, a new 3xx shape cast product realizes a bend angle of at least 36.5°.v. Product Form and Applications

[0066] As noted above, a new 3xx aluminum casting alloy may be in the form of an ingot, a billet, or a shape cast product. In one embodiment, a new 3xx aluminum casting alloy may be in the form of an ingot. In another embodiment, a new 3xx aluminum casting alloy may be in the form of a billet. In yet another embodiment, a new 3xx aluminum casting alloy may be in the form of shape cast product. As explained previously, the shape cast products may be used in any suitable application, including in any of an automotive, aerospace or industrial application.vi. Definitions

[0067] Temper definitions are per ANSI H35.1 (2009), entitled “American National Standard Alloy and Temper Designation Systems for Aluminum,” published by The Aluminum Association.

[0068] Strength and elongation are measured in accordance with ASTM E8 / E8M-21 and B557-15.

[0069] As used herein, “Quality Index” refers to a mechanical property that is calculated using the formula: Quality Index = Ultimate Tensile Strength (MPa) + 150*log(Elongation %).

[0070] As used herein, “shape cast product” means products that achieve their final or near final product form after the aluminum alloy casting process. A shape cast product is in final form if it requires no machining after casting. A shape cast product is in near final form if it requires some machining after casting. By definition, shape cast products excludes wrought products, which generally require hot and / or cold work after casting to achieve their final product form. Shape cast products may be produced via any suitable casting process, such as die casting and permanent mold casting processes, among others, as described in further detail below. As used herein, the term “shape cast product” excludes both ingot and billet, which are used for subsequent wrought aluminum alloy processing, i.e., ingot and billet are not a final product form.

[0071] As used herein, “megacastings” includes other terms known in the art, such as “gigacastings. ”Attorney Ref. No.: 169593.120026 / WOBRIEF DESCRIPTION OF DRAWINGS

[0072] FIGS. 1-4 are graphs illustrating the performance of various aluminum alloy products of Example 1.

[0073] FIG. 5 is a graph illustrating the performance of various aluminum alloy products of Example 2.

[0074] FIG. 6 illustrates the flow channels of the die used in Example 3.

[0075] FIG. 7 illustrates the flow lengths of various aluminum alloy products of Example 3.

[0076] FIG. 8 is a graph illustrating the performance of various aluminum alloy products of Example 4.

[0077] FIGS. 9A-9E are SEM images of various aluminum alloy products of Example 4.

[0078] FIGS. 10A-10B are XDS results of various aluminum alloy products of Example 4.

[0079] FIGS. 11A-11B are cross sectional images of SPR joint butts of various aluminum alloy products of Exam ple 7.

[0080] FIGS. 12-15 are graphs illustrating the performance of various aluminum alloy products of Example 9.

[0081] FIGS. 16-17 are graphs illustrating the performance of various aluminum alloy products of Example 10,

[0082] FIGS. 18-21 are graphs illustrating the performance of various aluminum alloy products of Example 11.

[0083] FIG. 22 is a perspective view of a megacasting for a vehicle.

[0084] FIGS. 23-27 illustrate exemplary method steps for producing various aluminum alloy products.DETAILED DESCRIPTION

[0085] Example 1 – Effect of Varying Silicon Content

[0086] Various 3xx aluminum alloys were cast into plates with dimensions of 80 mm (W) by 215 mm (L) by 3 mm (D) using a 280-ton vacuum assisted high pressure die casting (HPDC) machine. The compositions of the Example 1 alloys are shown in Table 1. Alloys A6-A10 were made partially with recycled material.Table 1 - Composition of Example 1 Alloys (all values in wt %) Alloy Si Fe Mn Mg Cr | Sr Ti Nb Al 6.73 0.15 0.54 0.12 0.02 0.076 — A2 8.01 0.14 0.54 0.12 0.02 0.073 —A3 9.13 0.14 0.52 0.11 0.01 0.07 —Attorney Ref. No.: 169593.120026 / WOA4 9.87 0.15 0.51 0.11 0.02 0.07 1 A5 9.87 0.15 0.51 0.11 0.02 0.07 0.05 A6 7.14 0.23 0.44 0.11 0.07 0.01 0.07! A7 8.12 0.25 0.44 0.14 0.07 0.01 0.07! A8 9.25 0.27 0.44 0.13 0.07 0.02 0.07 1 A9 10.11 0.23 0.39 0.14 0.06 0.01 0.07 1A 10 10.11 0.23 0.39 0.14 0.06 0.01 0.07 0.05

[0087] The balance of each alloy was aluminum, incidental elements and impurities, with no one impurity exceeding 0.05 wt. %, and with the total amount of impurities not exceeding 0.20 wt. %.

[0088] After casting, standard tensile specimens were taken from each as-cast plate, after which various properties of the alloys were tested, the results of which are provided in Table 2, below (values are the average of at least duplicate specimens). The mechanical properties were measured in accordance with ASTM B557-15.Table 2 Mechanical Properties of Example 1 AlloysUltimate TensileTensile Yield Elongation, QualityAlloy Strength Strength % Index (QI) (UTS), MPa (TVS), MPaAl 261 109 15.6 439A2 269 118 14.5 443A3 277 128 13.5 446A4 2.83 130 13.3 450A5 2.86 131 12.6 451A6 261 114 14.1 432A7 277 123 13.3 445A8 280 129 12.2 442A9 281 133 11.1 437A10 292 136 12.7 457

[0089] FIGS. 1-4 illustrate various properties of the alloys as a function of silicon and iron content. As shown in FIG. 1, both silicon content and iron content showed a significant impact on elongation. By increasing the silicon content from about 7 wt. % to about 10 wt. %, the elongation dropped from 15.5 %to 13.7 % for low iron content alloys (i.e., 0.15 wt. %Fe), and from about 14.1 % to about 11.1 % for high iron content alloys (i.e., 0.25 wt. % Fe). For every 1 wt. % increase of silicon, the elongation dropped about 1 % for high iron content alloys (i.e., 0.25 wt. % Fe). Increasing the iron content by about 0.1 wt. % may cause the elongation to drop by about 1 % for alloys with about 7 wt. % Si, and about 2 % for alloys with about 10 wt. % Si. HEIGHT="16" WIDTH="71" SRC="imgf000023_0001.tif" / >Attorney Ref. No.: 169593.120026 / WO

[0090] As shown in FIGS. 2-3, both tensile yield strength (TYS) and ultimate tensile strength (UTS) increase as the silicon content increases. For every 1 wt. % increase of silicon, the TYS and UTS increased by about 7 MPa on average.

[0091] As shown in FIG. 4, for low iron content alloys (i.e., 0.15 wt. % Fe), the quality index (QI) increased with the addition of silicon. When increasing the silicon content from about 7 wt. % to about 10 wt. %, the QI increased from 439 to 450. However, as also shown in FIG. 4, for high iron content alloys (i.e., 0.25 wt. % Fe), the QI increased and then decreased as the silicon content increased. By increasing the silicon content from about 7 wt. % to about 8 't. %, the QI increased from 432 to 445. However, by increasing the silicon content from about 8 wt. %to about 10 wt. %, the QI decreased from 445 to 437.

[0092] Example 2 - SPR Joining Performance of Example 1 Alloys

[0093] Various plates of Example 1 and a conventional C611 alloy plate were joined to a 1.4 mm HC340 steel sheet using a SH5.5 X 6.5-5 Sn self-piercing rivet (SPR) in six locations. The number of visible cracks on the joint buts were investigated and counted. The average number of cracks per SPR joint butt per alloy was calculated, the results of which are shown in Table 3, below. A maximum allowable number of minor cracks per SPR joint butt was set to 5. The C611 alloy is described, for instance, m U. S. Patent No. 6,773,666.Table 3 - Average Crackin per SPR Joint Butt of Example 1 Alloys Average Number of CracksAlloyper SPR Joint ButtAl 3A2 4.5A3 5A4 5.2A5 5.2A 6 2.7A7 5.0A8 5.8A9 5.3A10 6.8C611 4

[0094] FIG. 5 illustrates the average number ofcracks per SPR joint butt as a function of silicon and iron content. As shown in FIG. 5, both silicon content and iron content showed a significant impact on the average number of cracks per SPR joint butt. As silicon content increased, the average number of cracks per joint butt also increased. Additionally, alloys with higher iron content had a higher number of cracks per SPR joint butt. Only alloys Al, A2, A6, and the C611 alloy achieved an average number of minor cracks of less than 5 per SPR jointAttorney Ref. No.: 169593.120026 / WObut. Alloys AL A2, and A6 all also achieved an elongation of over 14 %. Additionally, alloys A 1 and A6 achieved a lower average number of cracks per joint butt compared to non-inventive alloy C611, even though alloys A l, A6, and C611 contained similar silicon content.

[0095] Example 3 - Flow length

[0096] Four additional 3xx aluminum alloys, all copper-free, were cast using a specially designed fluidity die. The composition and the casting temperature of the alloys are shown in Table 4,Table 4 - Composition and Casting Temperature of Example 3 Alloys(all composition values in wt. %)1 Casting Alloy Si Fe Mn Mg Sr Ti | Temperature | (°C) Bl 7.08 0.16 0.54 0.13 0.02 0.09 | 695 B2 8.05 0.16 0.53 0.13 0.02 0.09 690 B3 8.89 0.16 0.52 0.12 0.02 0.09 679B4 9.78 0.16 0.51 0.12 0.02 0.09 673

[0097] The balance of each alloy was aluminum, incidental elements and impurities, with no one impurity exceeding 0.05 wt. %, and with the total amount of impurities not exceeding 0.20 wt. %. The Example 3 alloys all contained not more than 0.01 wt. % Cu.

[0098] The fluidity mold had three different flow channels with dimensions (depth x width) of 10 x 6 mm, 4 mm, and 6 x 2 mm. The total lengths of the flow channels were 1469, 1726, and 2000 mm respectively. An image of the flow channels is shown in FIG. 6.

[0099] FIG. 7 illustrates the flow length as a function of silicon content and mold width. As may be appreciated from FIG. 7, alloys with higher silicon content were able to flow longer in the flow channels. The flow length increased in the 6 x 2 mm flow channel and the 8 x 4 mm flow channel when the silicon increased from approximately 7 wt. % to approximately 9 wt. % and increased even further when the silicon was increased to approximately 10 wt. %.

[0100] Flow lengths in the 8 x 4 mm flow channel were much longer than those in the 6 x 2 mm flow channel. It is believed that the flow lengths in the 6 x 2 mm flow channel were lower than the 8 x 4 mm flow channel because of the respective surface area to volume ratios (“SA: V ratio”). The 6 x 2 mm flow channel has a SA: V ratio of 1.33 and the 8 x 4 mm flow channel has a SA:V ratio of 0.75. Accordingly, it is believed that more heat was lost in the 6 x 2 mm flow' channel than the 8 x 4 mm flow channel because of the higher SA: V ratio which resulted in a lower flow length for alloys in the 6 x 2 mm flow' channel.

[0101] Example 4 - Effect of Varying Iron ContentAttorney Ref. No.: 169593.120026 / WO

[0102] Additional 3xx alloys, all copper free, were cast into plates with dimensions of 80 mm by 215 mm by 3 mm using a 280-ton vacuum assisted HPDC machine. The compositions of the Example 4 alloys are shown in Table 5.Table 5 - Composition of Example 4 Alloys (all values in wt. %) Alloy Si Fe Mn Mg Cr Ti SrCl 8.13 0.20 0.21 0.13 — 0.05 0.02 | C2 1 8.16 0.20 | 0.21 0.13 0.05 0.06 0.02 | C3 1 8.21 0.20 | 0.21 0.13 0.10 0.06 0.02 | C4 1 8.13 0.21 | 0.20 0.14 0.14 0.06 0.02 | C5 8.08 0.20 0.20 0.15 0.20 0.06 0.01 C6 1 8.47 0.17 | 0.41 0.13 — 0.07 0.01 | C7 1 8.35 0.17 | 0.40 0.13 0.06 0.07 0.01 | C8 i 8.39 0.17 j 0.39 0.13 0.10 0.07 0.02 j C9 i 8.34 0.18 | 0.39 0.13 0.15 0.07 0.02 |CIO i 8.34 0.18 | 0.39 0.13 0.18 0.07 0.02 |

[0103] The balance of each alloy was aluminum, incidental elements and impurities, with no one impurity exceeding 0.05 wt. %, and with the total amount of impurities not exceeding 0.20 wt. %. The Example 4 alloys all contained not more than 0.002 wt. % Cu.

[0104] After casting, standard tensile specimens were taken from each as-cast plate, after which various properties of the alloys were tested, the results of which are provided in Table 6A, below (values are the average of at least duplicate specimens). The mechanical properties were measured in accordance with ASTM B557-15.Table 6A - Mechanical Properties of Example 4 Alloys Elongation,Alloy UTS, MPa TYS, MPa QI%Cl 268 107 13.4 437C2 271 107 15.7 450C3 268 107 15.0 444C4 270 110 16.3 451C5 271 115 14.1 443C6 271 117 13.8 442C7 268 115 14.7 442C8 271 116 15.1 448C9 272 116 14.1 445CIO 271 115 14,8 447

[0105] FIG. 8 illustrate the elongation of the alloys as a function of chromium and manganese content. As shown in FIG. 8, both chromium and manganese showed a significant impact on elongation. Increasing the chromium content by 0.14 wt, % in alloys with 0.2. wt. % Mn increased the elongation from 13.4 % to 16.3 %. This is over a 20 % improvement.Attorney Ref. No.: 169593.120026 / WOIncreasing the chromium content by 0.1 wt. % in alloys with 0.4 wt. % Mn increased the elongation from 13.8 % to 15.1 %. It is believed that further increases of chromium will decrease the elongation due to the formation of an excess amount of intermetallic compounds.

[0106] FIGS. 9A-9E illustrate scanning electron microscope (SEM) images of alloys Cl- C5. As shown in FIGS. 9A-9E, the chromium content has a significant impact on the morphology of the alloy s. As the chromium content increases, the morphology of the iron- containing intermetallic particles gradually changed from a long needle shape (FIG. 9 A), to a round-ended rod shape (FIG. 9B), and to a polygonal shape (FIGS. 9C-9E). As the chromium content increases, the aspect ratio of the iron-containing intermetallic particles approaches 1 (L / W approaches 1). Iron-containing intermetallic particles with a low aspect ratio are less detrimental to mechanical properties, particularly elongation. Conversely, further increases in chromium content will lead to a higher quantity of intermetallic particles, which negatively affects elongation.

[0107] FIGS. 10A-10B illustrate Electron Dispersive X-Ray (EDS) images of alloys Cl and C4. Tables 6B-6C show the composition of EDS spot 1 of FIG. 10A and the composition of EDS spot 1 of FIG. 10B. As shown in FIGS. 10A-10B and in Tables 6B-6C below, the spots identified in the EDS images contain a large amount of aluminum, with identifiable peaks of silicon, manganese, chromium, and iron. Accordingly, FIGS. 10A-10B and Tables 6B-6C confirm the identified spots discussed relative to FIGS. 9A-9E above are intermetallic particles. Notably, the intermetallic particles of FIG. 10B are FeMnCr intermetallic particles.Table 6B - Composition of EDS Spot 1 (FIG. 10A)Element wt. % Atomic %Fe 0.8 0.4Al 80.9 83.2Si 14.8 14.6Cr 0.5 0.3Mn 3.1 1.6Table 6C - Composition of EDS Spot 1 (FIG. 10B)Element 1 wt. % 1 Atomic %Fe 2.0 1.1Al | 63.0 | 72.8Si | 10.9 | 12.1Cr | 10.8 | 6.5Mn i 13.2 i 7.2

[0108] Example 5 - Effect of Varying Vanadium, Zirconium, and BoronAttorney Ref. No.: 169593.120026 / WO

[0109] Six additional 3xx aluminum alloys, all copper-free, were made in accordance with the alloys of Example 1 above, the compositions of which are shown in Table 7.Table 7 - Composition of Example 5 Alloys (all values in wt. %) Alloy Si Fe Mn Mg Cr | Zn Ti Sr Zr V Cll 8.19 0.19 0.20 0.13 0.15 | 0.01 0.07 0.01 — 0.05 C12 8.02 0.18 0.20 0.13 0.15 | - 0.07 0.02 0.06 0.05 C13 8.09 0.18 0.19 0.13 0.15 | 0.03 0.07 0.02 0.10 0.05 C14 8.44 0.18 0.19 0.13 0.13 | - 0.06 0.02 0.01 Cl 5 8.21 0.17 0.19 0.13 0.16 | - 0.07 0.01 0.01Cl 6 8.17 0.16 0.19 0.12 0.15 | - 0.07 0.02 ~~ 0.01

[0110] The balance of each alloy was aluminum, incidental elements and impurities, with no one impurity exceeding 0.05 wt. %, and with the total amount of impurities not exceeding 0.20 wt. %. The Example 5 alloys all contained not more than 0.002 wt. % Cu. All Example 5 alloys contained approximately 0.0002 wt. % B, except alloy C16 which contained 0.0011 wt.

[0111] After casting, standard tensile specimens were taken from each as-cast plate, after which various properties of the alloys were tested, the results of which are provided in Table 8, below (values are the average of at least duplicate specimens). The mechanical properties were measured in accordance with ASTM B557-15.Table 8 - Mechanical Properties of Example 5 AlloysElongationAlloy UTS, MPa TYS, MPa, % QiCll 266 114 14.1 438 C12 271 116 14.3 443 Cl 3 265 112 14.2 438 Cl 4 264 112 14.7 438 C15 262 112 15.4 440C16 260 113 15.9 440

[0112] As shown in Table 8, the addition of vanadium and zirconium had no meaningful impact on the mechanical properties of alloys Cl 1-C13.

[0113] As shown in Table 8, boron may have a significant impact on the elongation of the alloys. Increasing the boron content from about 0.0002. wt. % to 0.0011 wt. % resulted in an increase in elongation of from 14.7 % to 15.9 % tor these alloys.

[0114] Example 6 - Bend Testing Example 4 and Example 5 / Alloys

[0115] Various plates of alloys of Examples 4 and 5 (e.g., alloys C1-C15) underwent a three-point bending test, according to VDA 238-100-2010. The results of the bending test are summarized in Table 9 below.Attorney Ref. No.: 169593.120026 / WOTable 9 - Bending Angles of Example 4 and Example 5 AlloysVDA 238-100-2010,AlloyBending Angle (°)Cl 36.8C2 34.9C3 35.1C4 33.6C5 32.0C6 31.8C7 34.4C8 32.6C9 33.2CIO 33.1CH 35.8C12 32.5Cl 3 33.9Cl 4 36.4C15 36.2

[0116] As may be seen from Table 9 above, the average bending angles are between 32 to 37 degrees for the alloys of Examples 4 and 5.

[0117] Example 7 - SPR Testing for Example 4 and Example 5 Alloys

[0118] Various plates of Example 4 and 5 alloys were subsequently joined to a 1.5 mm HC340 steel sheet with a HD3 5.2 X 5.4 self-piercing rivet (SPR) in five locations. Two different bottom dies were used with internal diameters of 11.1 mm and 12.4 mm, respectively. The outer diameter of the rivet punch used was 14.3 mm, When the bottom die with an internal diameter of 11.1 mm was used, severe cracking was formed in all of the alloys. When the bottom die with an internal diameter of 12.4 was used, acceptable SPR joint butts were obtained for all invention alloys (e.g., less than 5 minor cracks per SPR joint butt were observed on average).

[0119] FIGS. 11A-11B show a cross section of the SPR joint buts with two different bottom dies. As shown in FIG. 11 A, a SPRjoint butt with a bottom die with an internal diameter of 12.4 mm may produce a SPR joint butt with no observable cracks. As shown in FIG. 11B, an SPR joint butt with a bottom die with an internal diameter of 11.1 mm may produce an observable gap in between the alloy and the SPR.

[0120] Example 8 - Validation of Recycle Content

[0121] A 3xx aluminum alloy with high recycle content was cast into a plate with dimensions of 80 mm by 215 mm by 3 mm using a 280-ton vacuum assisted HPDC machine. The composition of the Example 8 alloy is shown in Table 10. The alloy was made with 92.85Page 29 of 48Attorney Ref. No.: 169593.120026 / WOwt. % recycle content, of which 21.85 % was from recycled die casting scrape (gating system) and 71 % was made from recycled Ixxx toothpaste tube.Table 10 - Composition of the Example 8 Alloy (ail values in wt. %) Alloy C17Si 8.26Fe 0.18Cu 0.01Mn 0.20Mg 0.13Cr 0.16Zn 0.09Ti 0.07Sr 0.02

[0122] The balance of the alloy was aluminum, incidental elements and impurities, with no one impurity exceeding 0.05 wt. %, and with the total amount of impurities not exceeding 0.20 wt. %.

[0123] After casting, standard tensile specimens were taken from the as-cast plate, after which various properties of the alloy were tested, the results of which are provided in Table 11, below (values are the average of at least duplicate specimens). The mechanical properties were measured in accordance with ASTM B557-15.Table 11 - Mechanical Properties of the Example 8 Alloy Alloy UTS, MPa TYS, MPa Elongation, % QIC17 259 109 16.4 440

[0124] As may be appreciated from Table 11 above, alloy Cl 7 was able to achieve similar UTS, TYS, elongation, and QI, as compared to other alloys that were created without recycled material. That is, an alloy according to the present disclosure made from 92.85 % recycled content was able to achieve similar mechanical properties as other alloys without recycled material or with less recycled material.

[0125] Example 9 – Effect of Varying Copper and Zinc Content

[0126] Various 3xx aluminum alloys were cast into plates with dimensions of 80 mm by 215 mm by 3 mm using a 280-ton vacuum assisted HPDC. The compositions of the Example 9 alloys are shown in Table 12.Table 12 - Composition of Example 9 Alloys (all values in wt. %) Alloy Si Fe Cu Mn Mg Cr Zn Zr C18 8.26 0.17 — 0.20 0.11 0.15 — 0.004Cl 9 8.40 0.17 0.09 0.20 0.13 0.16 0.01 0.004Attorney Ref. No.: 169593.120026 / WOC20 8.32 0.17 0.09 0.20 0.13 0.16 0.06 0.004 C21 8.24 0.19 0.06 0.25 0.16 0.16 0.23 0.024 C22 8.17 0.17 0.06 0.20 0.12 0.16 0.37 0.004 C23 8.10 0.19 0.07 0.26 0.16 0.15 0.56 0.024 C29 7.53 0.17 — 0.21 0.14 0.17 0.02C30 8.27 0.16 0.10 0.21 0.14 0.16 0.38C31 8.20 0.19 0.20 0.20 0.13 0.15 0.30 —C32 8.41 0.20 0.31 0.21 0.13 0.15 0.30 —C33 8.26 0.20 0.50 0.20 0.13 0.15 0.29 —

[0127] The balance of each of the alloys was aluminum, incidental elements and impurities, with no one impurity exceeding 0.05 wt. %, and with the total amount of impurities not exceeding 0.20 wt. %. All alloys of Table 12 contained about 0.06-0.08 wt. % Ti and about 0.01-0.02 wt. % Sr.

[0128] After casting, standard tensile specimens were taken from each as-cast plate, after which various properties of the alloys were tested, the results of which are provided in Table 13, below (values are the average of at least duplicate specimens). The mechanical properties were measured in accordance with ASTM B557-15.Table 13 — Mechanical Properties of Example 9 Alloys Elongation,Alloy UTS, MPa TYS, MPa QI%C18 254 109 14.6 429C19 261 109 15.0 437C20 256 108 14.2 429C21 265 113 14.9 441C22 259 109 15.3 437C23 267 116 13.3 436C29 254 108 15.7 433C30 265 112 16.3 446C31 266 112 15.1 443C32 272 115 15.5 451C33 278 117 14.6 452

[0129] FIGS. 12-13 illustrate various properties of the alloys as a function of copper. As shown in FIG. 12, increasing the copper content will increase the as-cast TYS. As shown by FIG. 13, increasing the copper content will also decrease the elongation. It is also noted that if the copper content is increased above 0.5 wt. % the tendency of the alloys to hot crack will significantly increase and the corrosion resistance will decrease.

[0130] FIGS. 14-15 illustrate various properties of the alloys as a function of zinc.. As shown in FIG. 14, a small increase in the zinc content increased the elongation. However, as also shown in FIG. 14, if the amount of zinc is too large (e.g., greater than 0.5 wt. %), theAttorney Ref. No.: 169593.120026 / WOelongation will decrease. As shown by FIG. 15, increasing the zinc content will increase the as-cast TYS.

[0131] Example 10 -- Effect of Varying Iron content

[0132] V arious 3xx alloys, all copper free, were cast into plates with dimensions of 80 mm by 215 mm by 3 mm using a 280-ton vacuum assisted HPDC machine. The compositions of tire Example 10 alloys are shown in Table 14.Table 14 - Composition of Example 10 Alloys (all values in wt. %) Alloy Si Fe Mn Mg Cr Zn C24 8.33 0.18 0.21 0.15 0.15 0.02 C25 8.19 0.26 0.21 0.15 0.15 0.02 C26 8.17 0.35 0.21 0.13 0.15 0.02 C27 8.07 0.43 0.21 0.13 0.15 0.03 C28 8.18 0.52 0.21 0.13 0.15 0.04 C34 8.29 0.19 0.20 0.16 0.15 --C35 8.24 0.91 0.22 0.16 0.14 --C36 8.32 1.09 0.21 0.15 0.14 --C37 8.22 1.31 0.21 0.15 0.13 --C38 8.29 1.51 0.21 0.15 0.14 --C39 8.19 1.79 0.22 0.14 0.15 --

[0133] The balance of each alloy was aluminum, incidental elements and impurities, with no one impurity exceeding 0.05 wt. %, and with the total amount of impurities not exceeding 0.20 wt. %. The Example 3 alloys all contained not more than 0.01 wt. % Cu. All alloys of Table 14 contained about 0.06-0.07 wt. % Ti and about 0.02 wt. % Sr.

[0134] After casting, standard tensile specimens were taken from each as-cast plate, after which various properties of the alloys were tested, the results of which are provided in Table 15, below (values are the average of at least duplicate specimens). The mechanical properties were measured in accordance with ASTM B557-15.Table 15 - Mechanical Properties of Example 10 Alloys Elongation,Alloy UTS, MPa TYS, MPa% QIC24 265 115 15.2 442C25 257 111 14.3 430C26 262 112 15.5 441C27 258 112 15.3 436C28 256 109 15.2 433C34 271 110 16.4 453C35 279 115 12.8 445C36 276 112 12.1 438C37 276 111 11.8 437Attorney Ref. No.: 169593.120026 / WOC38 276 117 10.3 428C39 274 119 9.4 420

[0135] FIGS. 16-17 show various properties of the alloys as a function of iron. As shown in FIG. 16, as the iron content increases, the elongation decreases. However, even with an iron content of over 1.5 wt. %, an elongation of over 10 %may still be achieved. As shown in FIG.17, as the iron content increases, the as-cast. TYS increases.

[0136] Example 11 - Effect of Varying Magnesium Content

[0137] Various 3xx aluminum alloys were cast into plates with dimensions of 80 mm by 215 mm by 3 mm using a 280-ton vacuum assisted HPDC machine. The compositions of the Example 11 alloys are shown in Table 16.Table 16 - Composition of Example 11 Alloys (all values in wt. %) Alloy Si Fe Cu Mn Mg Cr Zn C40 8.60 0.24 0.08 0.21 0.14 0.15 0.08 C41 8.55 0.24 0.08 0.21 0.21 0.15 0.08 C42 8.48 0.24 0.08 0.21 0.33 0.15 0.08 C43 8.51 0.24 0.08 0.21 0.43 0.15 0.08 C44 8.44 0.24 0.08 0.21 0.52 0.15 0.08 C45 8.41 0.25 0.08 0.21 0.63 0.15 0.08 C46 8.36 0.25 0.08 0.21 0.71 0.15 0.08C47 8.36 0.25 0.08 0.21 0.81 0.15 0.08

[0138] The balance of each alloy was aluminum, incidental elements and impurities, with no one impurity exceeding 0.05 wt. %, and with the total amount of impurities not exceeding 0.20 wt. %. All alloys of Table 16 contained about 0.08 wt. % Ti and about 0.02 wt. % Sr.

[0139] After casting, standard tensile specimens were taken from each as-cast plate, after which various properties of the alloys were tested, the results of which are provided in Table 17, below (values are the average of at least duplicate specimens). The mechanical properties were measured in accordance with ASTM B557-15.Table 17 - Mechanical Properties of Example 11 Alloys Allo Elongation,UTS, MPa TYS, MPa Qiy _C40 281 117 14.3 454C41 285 121 14.5 459C42 294 128 13.4 463C43 298 134 12.1 461C44 301 134 12.2 464C45 301 128 9.3 446C46 301 139 7.1 428C47 321 159 7.2 450Attorney Ref. No.: 169593.120026 / WO

[0140] FIGS. 18-21 show various properties of the alloys as a function of magnesium. As shown in FIG. 18 the magnesium content has a significant impact on elongation. By increasing the magnesium content about 0.1 wt. %, the elongation will decrease by about 0.7 %. As shown in FIG. 19, the magnesium content has a significant impact on the TYS. By increasing the magnesium content about 0.1 wt. %, the as-cast TYS will increase by about 5 MPa. As shown in FIG. 20, the magnesium content has a significant impact on the UTS. By increasing the magnesium content about 0.1 wt. %, the as-cast UTS will increase by about 5 MPa. As shown by alloy C44, an alloy with 0.5 wt. % Mg may achieve a 300 MPa UTS, a 135 MPa TYS, and an elongation of over 12 %.

[0141] As shown in FIG. 21, the QI varies with the magnesium content. A slight increase in magnesium from about 0.2 % to about 0.4 or 0.5 wt. % will increase the QI. However, increasing the magnesium content to above 0.6 wt. % will decrease the QI.

[0142] Example 12 - Investigation of Thermal Stability

[0143] Various plates of Examples 4 and 5 were artificially aged at 195° C for 45 minutes. Then, standard tensile specimens were taken from each aged plate, after which various properties of the alloys were tested, the results of which are provided in Tables 18-21, below. The artificially aged alloys are the “Aged” alloys in Tables 18-21. The properties of the “Aged” alloys are compared to a second set of plates of Examples 4 and 5 alloys that were not aged or that were naturally aged for less than two days. The alloys that were not aged or naturally aged for less than two days are the “As-Cast” alloys in Tables 18-21. The mechanical properties were measured in accordance with ASTM B557-15.Table 18 - Ultimate Tensile Strength for As-Cast and Aged Alloys (MPa)DifferenceAlloy As- Cast Aged (Aged ■■■ As- Cast)Cl 264 267C2 270 273 3 C3 269 268 -1 C4 269 271 7 C5 268 273 4 C6 272 277 5 C7 266 272 6 C8 268 269 1 C9 269 272 7 CIO 270 272 2 CH 268 274 6 C12 268 274 6C13 274 278 5Attorney Ref. No.: 169593.120026 / WOC14 261 264 2C15 260 263 3C16 261 265 3Table 19 - Tensile Yield Strength for As-Cast and Aged Alloys (MPa)Difference Alloy As-Cast Aged (Aged - As- Cast)Cl 109 131 22C2 111 135 2.3C3 112 131 19C4 115 134 19C5 116 136 20C6 122 142 20C7 117 136 19C8 119 136 17C9 120 144 23CIO 119 143 24Cl 1 119 141 22C12 119 138 19C13 121 142. 2.1C14 115 131 16C15 115 131 16Cl 6 113 131 18Table 20 - Elongation for As-Cast and Aged Alloys (%)| Difference Alloy As-Cast Aged | (Aged - As- | Cast)Cl 14.5 11.8 | -2.7C2 15.8 12.5 | -3.3C3 15.2 12.7 | -2.5C4 16.5 12.9 | -3.6C5 14.5 14,9 0.4C6 14.6 13.2 -1.4C7 15.4 14.1 | -1.3C8 14.8 14.4 | -0.4C9 14.4 14.5 | 0.1CIO 14.5 12.4 -2.1Cl 1 14.6 13.3 -1.2C12 14.5 13.9 | -0.7C13 14,7 13.1 | -1.6C14 14.9 15.3 | 0.4C15 14.9 13.5 | -1.5Cl 6 15.6 15.5 | -0.1Attorney Ref. No.: 169593.120026 / WOTable 21 - Quality Index for As-Cast and Aged AlloysDifferenceAhoy As- Cast Aged (Aged - As- Cast)Cl 439 428 -11 C2 449 437 -12 C3 446 434 -13 C4 452 438 -14 C5 443 449 6 C6 446 445 -2 C7 443 444 0 C8 444 443 -1 C9 443 446 3 C10 444 436 -8 Cll 442 442 0 C12 441 445 4 C13 449 446 -3 Cl 4 436 441 5 C15 436 432 -4C16 440 443

[0144] As shown in Tables 18-21, artificial aging may improve tensile yield strength with negligible or small effects on elongation.

[0145] In a different aging test, various plates of Examples 4 and 5 were naturally aged for different periods of times. Standard tensile specimens were taken from each aged plate, after which various properties of the alloys were tested, the results of which are provided in Tables 22-37 below. The properties of the various aged alloys were compared to other standard tensile specimens from other plates of the same composition that were natural aged for different times. The mechanical properties were measured in accordance with ASTM B557-15.Table 22 - Mechanical Properties of Alloy Cl for Various Natural Aging Times Days Aged UTS, MPa TVS, MPa Elongation, % QI7 260 107 13.6 43043 269 112 15.5 447 Table 23 - Mechanical Properties of Alloy C2 for Various Natural Aging Times Days Aged UTS, MPa TVS, MPa Elongation, % QI2 267 110 16.4 44943 272 113 15.2 449 Table 24 - Mechanical Properties of Alloy C3 for Various Natural Aging Times Days Aged UTS, MPa TYS, MPa Elongation, % QI2 265 110 14.6 440Attorney Ref. No.: 169593.120026 / WO43 273 115 15.8 453 Table 25 - Mechanical Properties of Alloy C4 for Various Natural Aging Times Days Aged UTS, MPa TYS, MPa i Elongation, % QI 1 2 2.66 112 | 17.1 450 |43 273 117 | 16.0 453 | Table 26 - Mechanical Properties of Alloy C5 for Various Natural Aging TimesDays Aged UTS, MPa TYS, MPa Elongation, % QI2 266 114 14.1 43843 274 121 15.5 452 Table 27 - Mechanical Properties of Alloy C6 for Various Natural Aging Times Days Aged UTS, MPa TYS, MPa Elongation, % QI1 267 119 14.7 44240 282 128 14.3 456 Table 28 - Mechanical Properties of Alloy C7 for Various Natural Aging Times Days Aged UTS, MPa TYS, MPa Elongation, % Qi1 263 117 15.1 43940 271 119 16.0 451 Table 29 - Mechanical Properties of Alloy C8 for Various Natural Aging Times Days Aged UTS, MPa TYS, MPa Elongation, % QI7 266 119 15.0 443 7 269 119 13.3 4378 270 119 15.6 449 Table 30 - Mechanical Properties of Alloy C9 for Various Natural Aging Times Days Aged UTS, MPa TYS, MPa Elongation, % Qi1 265 119 13.8 435 6 272 119 14.6 4469 272 122 14.9 448 Table 31 - Mechanical Properties of Alloy C10 for Various Natural Aging Times Days Aged UTS, MPa TYS, MPa Elongation, % Qi1 266 119 15.6 445 6 269 117 14.3 4429 274 120 13.7 444 Table 32 - Mechanical Properties of Alloy Cll for Various Natural Aging Times Days Aged UTS, MPa TYS, MPa Elongation, % Qi1 263 119 14.0 435 5 262 115 13.7 4338 278 123 16.0 458 Table 33 - Mechanical Properties of Alloy C12 for Various Natural Aging Times Davs AgedAttorney Ref. No.: 169593.120026 / WO1 263 121 14.2 435 5 268 117 13.0 4348 273 119 16.5 455 Table 34 - Mechanical Properties of Alloy C13 for Various Natural Aging Times Days Aged UTS, MPa TYS, MPa Elongation, % QI1 271 122 14.7 446 5 275 119 14.5 4498 276 122 14.9 451 Table 35 - Mechanical Properties of Alloy C14 for Various Natural Aging Times Days Aged UTS, MPa TYS, MPa Elongation, % QI1 259 117 15.7 439 4 259 111 12.7 42438 266 117 16.2 447 Table 36 - Mechanical Properties of Alloy C15 for Various Natural Aging Times Days Aged UTS, MPa TYS, MPa | Elongation, % QI 1 1 255 116 | 15.5 433 | 4 262 112 1 13.3 430 138 264 116 i 16.0 444 i Table 37 - Mechanical Properties of Alloy C16 for Various Natural Aging Times Days Aged UTS, MPa TYS, MPa Elongation, % Qi1 260 113 15.9 440 4 260 111 14.6 4357 263 114 16.4 445

[0146] As shown in Tables 22-37, natural aging may improve TYS, UTS, and elongation. It is believed that the elongation, UTS, and TYS all increase after the first seven days of naturally aging because the microstructure becomes more stabilized due to the growth and coarsening of precipitates which reduces the internal stresses.[01471 Example 13 - Production of Megacasting

[0148] Alloy C17 is cast using a 9,000-ton HPDC machine to create a megacasting. The machine uses a mold that is a megacasting mold. The megacasting mold is used to create a megacasting.

[0149] FIG. 22 illustrates an example image of a megacasting that could be created using a 9,000 ton HPDC machine. As shown in FIG. 22, the megacasting has multiple arcuate surfaces and multiple sloped surfaces. While the megacasting is a monolithic, single-piece casting, it includes a variety of shape and non-uniform geometric structures. The megacasting may be secured to one or more structures including one or more automobile structures. TheAttorney Ref. No.: 169593.120026 / WOmegacasting may be attached to other structures with the use of rivets, welding, and other methods.

[0150] In one embodiment, a megacasting, such as that illustrated in FIG, 22, is produced using any of the aluminum alloy compositions described herein. After casting, a visual inspections of the megacasting reveals no visual defect, and ultrasonic or other suitable testing of the megacasting reveals the absence of any substantial porosity. The megacasting also realizes an improved combination of elongation, bend angle, and / or strength, among other properties. The megacasting may be shipped in an as-cast or naturally aged condition.

[0151] The megacasting is a single cast product that contains 40 or more components. Traditional methods of creating the 40 or more components requires casting individual products and using a method of joining them. The production of a megacasting with a single megacasting mold reduces the manufacturing time, the CO₂ output, and manufacturing costs, among other things. Additionally, the creation of a megacasting with a single megacasting mold increases the uniformity of final product and the customizability of the products, among other things.

[0152] These and other aspects, advantages, and novel features of this new technology are set forth in part in the description and figures herein and will become apparent to those skilled in the art upon examination of the description and figures herein, or may be learned by practicing one or more embodiments of the technology provided for by the present disclosure.

[0153] The present disclosure was explained, in part, with reference to the attached drawings, wherein like structures are referred to by like numerals throughout the several views. The drawings shown are not necessarily to scale, with emphasis instead generally being placed upon illustrating the principles of the present disclosure. Further, some features may be exaggerated to show details of particular components. In addition, any measurements, specifications and the like shown in the figures are intended to be illustrative, and not restrictive. Therefore, specific structural and functional details disclosed herein are not to be interpreted as limiting, but merely as a representative basis for teaching one skilled in the art to variously employ the present disclosure.

[0154] Among those benefits and improvements that have been disclosed, other objects and advantages of this invention will become apparent from the description figures herein. Detailed embodiments of the present invention are disclosed herein; however, it is to be understood that the disclosed embodiments are merely illustrative of the invention that may be embodied in various forms. In addition, each of the examples given in connection with the various embodiments of the invention is intended to be illustrative, and not restrictive. Therefore,Attorney Ref. No.: 169593.120026 / WOspecific structural and functional details disclosed herein are not to be interpreted as limiting, but merely as a representative basis for teaching one skilled in the art to variously employ the present disclosure.

[0155] Throughout the specification and claims, the following terms take the meanings explicitly associated herein, unless the context clearly dictates otherwise. The phrases “in one embodiment” and “in some embodiments” as used herein do not necessarily refer to the same embodiment(s), though they may. Furthermore, the phrases “in another embodiment,” “in yet another embodiment,” and “in some other embodiments” as used herein do not necessarily refer to a different embodiment, although they may. Thus, various embodiments of the invention may be readily combined, without departing from the scope or spirit of the invention.

[0156] In addition, as used herein, the term “or” is an inclusive “or” operator, and is equivalent to the term “and / or,” unless the context clearly dictates otherwise. The term “based on” is not exclusive and allows for being based on additional factors not described, unless the context clearly dictates otherwise. In addition, throughout the specification, the meaning of “a,” “an,” and “the” include plural references, unless the context clearly dictates otherwise. Tire meaning of “in” includes “in” and “on”, unless the context clearly dictates otherwise.

[0157] While a number of embodiments of the present invention have been described, it is understood that these embodiments are illustrative only, and not restrictive, and that many modifications may become apparent to those of ordinary skill in the art. However, it is to be expressly understood that such modifications and adaptations are within the spirit and scope of the present disclosure. Further still, unless the context clearly requires otherwise, the various steps may be carried out in any desired order, and any applicable steps may be added and / or eliminated.

Claims

Attorney Ref. No.: 169593.120026 / WOCLAIMSWhat is claimed is:

1. A 3 xx aluminum casting alloy comprising:from 7.0 to 9.0 wt. % Si;from 0.05 to 0.6 wt. % Mg;from 0.1 to 0.4 wt. % Mn;from 0.05 to 0.25 wt. % Cr;wherein (wt. % Mn) + (wt. % Cr) is from 0.2 to 0.6 wt. %;from 0.05 to 1.5 wt. % Fe;up to 0.5 wt. % Cu;up to 0.5 wt. % Zn;up to 0.15 wt. % Ti;up to 0.15 wt. % V;up to 0.15 wt, % Zr; andup to 0.05 wt. % of any one of Sr, Sb, Na, Ca;the balance being aluminum, optional incidental elements and impurities; wherein the 3xx aluminum casting alloy is in a form of an ingot, billet or a shape cast product.

2. The 3xx aluminum casting alloy of claim 1, wherein the 3xx aluminum casting alloy includes at least 7.1 wt. % Si, or at least 7.2 wt. % Si, or at least 7.3 wt. % Si, or at least 7.4 wt. % Si, or at least 7.5 wt. % Si, or at least 7.6 wt. % Si, or at least 7.7 wt. % Si, or at least 7.8 wt. % Si, or at least 7.9 wt. % Si, or at. least 8.0 wt. % Si, or at. least 8.1 wt. % Si, or at least. 8.2 wt. % Si, or at least 8.3 wt. % Si, or at least 8.4 wt. % Si.

3. The 3xx aluminum casting alloy of any of the preceding claims, wherein the 3xx aluminum casting alloy includes not greater than 8.9 wt. % Si, or not greater than 8.8 wt. % Si, or not greater than 8.7 wt. % Si, or not greater than 8.6 wt. % Si.

4. The aluminum alloy of any of the preceding claims, wherein the 3xx aluminum casting alloy includes at least 0.07 wt. % Mg, or at least 0.09 wt. % Mg, or at least 0.11 wt. % Mg, or at least 0.13 wt. % Mg, or at least 0.15 wt. % Mg, or at least 0.17 wt. % Mg, or at least 0.19 wt. % Mg, or at least. 0.20 wt. % Mg.

5. The 3xx aluminum casting alloy of any of the preceding claims, wherein the 3xx aluminum casting alloy includes not greater than 0.55 wt. % Mg, or not greater than 0.50 wt, % Mg, or not greater than 0.45 wt. % Mg, or not greater than 0.40 wt. % Mg, or not greater than 0.35 wt.Attorney Ref. No.: 169593.120026 / WO% Mg, or not greater than 0.30 wt. % Mg, or not greater than 0.25 wt. % Mg, or not greater than 0.20 wt. % Mg, or not greater than 0.15 wt. % Mg.

6. The 3xx aluminum casting alloy of any of the preceding claims, wherein the 3xx aluminum casting alloy includes at least 0.12 wt. % Mn, or at least 0.14 wt. % Mn, or at least 0.16 wt. % Mn, or at least 0.18 wt. % Mn.

7. The 3xx aluminum casting alloy of any of the preceding claims, wherein the 3xx aluminum casting alloy includes not greater than 0.38 wt. % Mn, or not greater than 0.36 wt. % Mn, or not greater than 0.34 wt. % Mn, or not greater than 0.32 wt. % Mn, or not greater than 0.30 wt. % Mn, or not greater than 0.28 wt. % Mn, or not greater than 0.26 wt. % Mn, or not greater than 0.24 wt. % Mn, or not greater than 0.22 wt. % Mn.

8. The 3xx aluminum casting alloy of any of the preceding claims, wherein the 3xx aluminum casting alloy includes at least 0.07 wt. % Cr, or at least 0.09 wt. % Cr, or at least 0.11 wt. % Cr, or at least 0.13 wt. % Cr.

9. The 3xx aluminum casting alloy of any of the preceding claims, wherein the 3xx aluminum casting alloy includes not greater than 0.23 wt. % Cr, or not greater than 0.21 wt. % Cr, or not greater than 0.19 wt. % Cr, or not greater than 0.17 wt. % Cr.

10. The 3xx aluminum casting alloy of any of the preceding claims, wherein the 3xx aluminum casting alloy includes at least 0.22 ((wt. % Mn) + (wt, % Cr)), or at least 0,2.4 ((wt. % Mn) + (wt. % Cr)), or at least 0.26 ((wt. % Mn) (wt. % Cr)), or at least 0.28 ((wt. % Mn) + (wt. % Cr)), or at least 0.30 ((wt. % Mn) + (wt. % Cr)), or at least 0.32 ((wt. % Mn) + (wt. % Cr)), or at least 0.34 ((wt. % Mn) + (wt. % Cr)).

11. The 3xx aluminum casting alloy of any of the preceding claims, wherein the 3xx aluminum casting alloy includes not greater than 0.55 wt. % ((wt. % Mn) 4- (wt. % Cr)), or not greater than 0.50 wt. % ((wt. % Mn) + (wt. % Cr)), or not greater than 0.45 wt. % ((wt. % Mn) + (wt. % Cr)), or not greater than 0.40 wt, % ((wt. % Mn) + (wt. % Cr)), or not greater than 0.35 wt, % ((wt, % Mn) + (wt. % Cr)).

12. The 3xx aluminum casting alloy of any of the preceding claims, wherein the 3xx aluminum casting alloy includes at least 0.07 wt. % Fe, or at least 0.09 wt. % Fe, or at least 0.11 wt. % Fe, or at least 0.13 wt. % Fe, or at least 0.15 wt. % Fe, or at least 0.17 wt. % Fe, or at least 0.19 wt. % Fe, or at least 0.21 wt. % Fe, or at least 0.23 wt. % Fe.

13. The 3xx aluminum casting alloy of any of the preceding claims, wherein the 3xx aluminum casting alloy includes not greater than 1.4 wt. % Fe, or not greater than 1,3 wt. % Fe, or not greater than 1.2 wt, % Fe, or not greater than 1.1 wt, % Fe, or not greater than 1.0 wt, % Fe, or not greater than 0.9 wt. % Fe, or not greater than 0.8 wt. % Fe, or not greater than 0.75 wt. %Attorney Ref. No.: 169593.120026 / WOFe, or not greater than 0.70 wt. %Fe, or not greater than 0.65 wt. %Fe, or not greater than 0.60 wt. % Fe, or not greater than 0.55 wt. % Fe, or not greater than 0.50 wt. % Fe, or not greater than 0.45 wt. % Fe, or not greater than 0.40 wt. % Fe, or not greater than 0,35 wt. % Fe, or not greater than 0.30 wt. % Fe.

14. The 3xx aluminum casting alloy of any of the preceding claims, wherein the 3xx aluminum casting alloy includes at least 0.02 wt. % Cu, or at least 0.04 wt. % Cu, or at least 0.06 wt. % Cu, or at least. 0.08 wt. % Cu, or at least. 0.10 wt, % Cu, or at least 0.12 wt. % Cu, or at least 0.14 wt. % Cu.

15. The 3xx aluminum casting alloy of any of the preceding claims, wherein the 3xx aluminum casting alloy includes not greater than 0.45 wt. % Cu, or not greater than 0.40 wt. % Cu, or not greater than 0.35 wt. % Cu, or not greater than 0.30 wt. % Cu, or not greater than 0.28 wt. % Cu, or not greater than 0.26 wt. % Cu, or not greater than 0.24 wt. % Cu, or not greater than 0.22 wt. % Cu, or not greater than 0.20 wt. % Cu, or not greater than 0.18 wt. % Cu, or not greater than 0, 16 wt. % Cu, or not greater than 0.14 wt. % Cu.

16. The 3xx aluminum casting alloy of any of the preceding claims, wherein the 3xx aluminum casting alloy includes at least 0.02 wt. % Zn, or at least 0.04 wt. % Zn, or at least 0.06 wt. % Zn, or at least 0.08 wt. % Zn.

17. The 3xx aluminum casting alloy of any of the preceding claims, wherein the 3xx aluminum casting alloy includes not greater than 0.55 wt. % Zn, or not greater than 0.50 wt. % Zn, or not greater than 0.45 wt. % Zn, or not greater than 0.40 wt. % Zn, or not greater than 0.35 wt. % Zn, or not. greater than 0.30 wt. % Zn, or not greater than 0.25 wt. % Zn, or not greater than 0.23 wt. % Zn, or not greater than 0.21 wt. % Zn, or not greater than 0.19 wt. % Zn, or not greater than 0.17 wt. % Zn, or not greater than 0.15 wt. % Zn, or not greater than 0.13 wt. % Zn, or not greater than 0.11 wt. % Zn, or not greater than 0.09 wt. % Zn.

18. The 3xx aluminum casting alloy of any of the preceding claims, wherein the 3xx aluminum casting ahoy includes at least 0.02 wt. % Cu and at least 0.02 wt. % Zn, or at least 0.08 wt. % Cu and at least 0.08 wt. % Zn, or at least 0.2 wt. % Cu and at least 0.2 wt. % Zn, or at least 0.2 wt. % Cu and at least 0.3 wt, % Zn.

19. The 3xx aluminum casting alloy of any of the preceding claims, wherein the 3xx aluminum casting alloy includes at least 0.005 wt. % Ti, or at least 0.01 wt. % Ti, or at least 0.015 wt. % Ti, or at least 0.

02. wt. % Ti, or at least 0.025 wt. % Ti, or at least 0.03 wt. % Ti, or at least 0.035 wt. % Ti, or at least 0.04 wt. % Ti, or at least 0.045 wt. % Ti, or at. least 0.05 wt. % Ti.

20. The 3xx aluminum casting alloy of any of the preceding claims, wherein the 3xx aluminum casting alloy includes not greater than 0.14 wt. % Ti, or not greater than 0.13 wt. % Ti, or notAttorney Ref. No.: 169593.120026 / WOgreater than 0.12 wt. % Ti, or not greater than 0.11 wt. % Ti, or not greater than 0.10 wt. % Ti, or not greater than 0.09 wt. % Ti, or not greater than 0.08 wt. % Ti.

21. The 3xx aluminum casting alloy of any of the preceding claims, wherein the 3xx aluminum casting alloy includes at least 0.005 wt. % V, or at least 0.01 wt. % V, or at least 0.015 wt. % V, or at least 0.02 wt. % V, or at least 0.025 wt. % V, or at least 0.03 wt. % V, or at least 0.035 wt. % V, or at least 0.04 wt. % V, or at least 0.045 wt. % V, or at least 0.05 wt. % V.

22. The 3xx aluminum casting alloy of any of the preceding claims, wherein the 3xx aluminum casting alloy includes not greater than 0.14 wt. % V, or not greater than 0.13 wt. % V, or not greater than 0.12 wt. % V, or not greater than 0.11 wt. % V, or not greater than 0.10 wt. % V, or not greater than 0.09 wt. % V, or not greater than 0.08 wt. % V.

23. The 3xx aluminum casting alloy of any of the preceding claims, wherein the 3xx aluminum casting alloy includes at least 0.005 wt. % Zr, or at least 0.01 wt. % Zr, or at least 0.015 wt. % Zr, or at least 0.02 wt. % Zr, or at least 0.025 wt. % Zr, or at least 0.03 wt. % Zr, or at least 0.035 wt. % Zr, or at least 0.04 wt. % Zr, or at least 0.045 wt. % Zr, or at least 0.05 wt.. % Zr.

24. The 3xx aluminum casting alloy of any of the preceding claims, wherein the 3xx aluminum casting alloy includes not greater than 0.14 wt. % Zr, or not greater than 0.13 wt. % Zr, or not greater than 0.12 wt. % Zr, or not greater than 0.11 wt. %Zr, or not greater than 0.10 wt. %Zr, or not greater than 0.09 wt. % Zr, or not greater than 0.08 wt. % Zr.

25. The 3xx aluminum casting alloy of any of the preceding claims, wherein the 3xx aluminum casting alloy includes at least 0.03 wt. % V and at least 0.03 wt. % Zr, or at least 0.05 wt. % V and at least 0.10 wt, % Zr.

26. The 3xx aluminum casting alloy of any of the preceding claims, wherein the 3xx aluminum casting alloy includes at least 50 ppm Sr, or at least 100 ppm Sr, or at least 150 ppm Sr, or at least 200 ppm Sr, or at least 2.50 ppm Sr, or at least 300 ppm Sr.

27. The 3xx aluminum casting alloy of any of the preceding claims, wherein the 3xx aluminum casting alloy includes at least 50 ppm Sb, or at least 100 ppm Sb, or at least. 150 ppm Sb, or at least 200 ppm Sb, or at least 250 ppm Sb, or at least 300 ppm Sb.

28. The 3xx aluminum casting alloy of any of the preceding claims, wherein the 3xx aluminum casting alloy includes at least 50 ppm Na, or at least 100 ppm Na, or at least 150 ppm Na, or at least 200 ppm Na, or at least 250 ppm Na, or at least 300 ppm Na.

29. The 3xx aluminum casting alloy of any of the preceding claims, wherein the 3xx aluminum casting alloy includes at least. 50 ppm Ca, or at least 100 ppm Ca, or at least 150 ppm Ca, or at least 200 ppm Ca, or at least 250 ppm Ca, or at least 300 ppm Ca.Attorney Ref. No.: 169593.120026 / WO30. The 3xx aluminum casting alloy of any of the preceding claims, wherein the 3xx aluminum casting alloy includes less than 0.04 wt. % Mo, or less than 0.01 wt. % Mo.

31. The 3xx aluminum casting alloy of any of the preceding claims, wherein the 3xx aluminum casting alloy includes less than 0.04 wt. % Li, or less than 0.01 wt. % Li.

32. The 3xx aluminum casting alloy of any of the preceding claims, wherein the 3xx aluminum casting alloy includes less than 0.04 wt. % Ag, or less than 0.01 wt. % Ag.

33. The 3xx aluminum casting alloy of any of the preceding claims, wherein the 3xx aluminum casting alloy includes less than 0.04 wt. % Pb, or less than 0.01 wt. % Pb.

34. The 3xx aluminum casting alloy of any of the preceding claims, wherein the 3xx aluminum casting alloy includes less than 0.04 wt. % Cd, or less than 0.01 wt. % Cd.

35. The 3xx aluminum casting alloy of any of the preceding claims, wherein the 3xx aluminum casting alloy includes less than 0.04 wt. % Sn, or less than 0.01 wt. % Sn.

36. The 3xx aluminum casting alloy of any of the preceding claims, wherein the 3xx aluminum casting alloy includes less than 0.04 wt. % Bi, or less than 0.01 wt, % Bi.

37. The 3xx aluminum casting alloy of any of the preceding claims, wherein the shape cast product comprises FeCrMn intermetallic particles.

38. The 3xx aluminum casting alloy of any of the preceding claims, wherein the 3xx aluminum casting alloy is made from at least 50 % recycled aluminum, or at least 55 % recycled aluminum, or at least 60 % recycled aluminum, or at least 65 % recycled aluminum, or at least 70 % recycled aluminum, or at least 75 % recycled aluminum, or at least 80 % recycled aluminum, or at least 85 % recycled aluminum, or at least 90 % recycled aluminum, or at least 95 % recycled aluminum.

39. A method of making a shape cast product of any of claims 1-38, comprising:(a) filling a shape casting mold with a molten aluminum alloy, where the molten aluminum alloy realizes the aluminum casting alloy composition of any of claims 1-38;(b) cooling the molten aluminum alloy composition within the shape casting mold, thereby forming a shape cast product.

40. The method of claim 39, herein the shape casting mold is a die casting mold.

41. The method of any of claims 39-40, w'herein the shape casting mold is a high pressure die casting mold.

42. The method of any of claims 39-41, comprising applying pressure to the mold or the molten aluminum alloy before, during, or after the cooling step (b).

43. The method of any of claims 39-42, wherein the shape casting mold is a megacasting mold and wherein the shape cast product is a megacastingAttorney Ref. No.: 169593.120026 / WO44. The method of any of claims 39-43, wherein the cooling step (b) comprises cooling the molten aluminum alloy composition to ambient temperature.

45. The method of any of claims 39-44, comprising:extracting the shape cast product from the shape casting mold.

46. The method of any of claims 39-45, wherein the shape cast product is substantially surface defect free.

47. The method of any of claims 39-46, wherein the shape cast product is substantially non-porous.

48. The method of any of claims 39-47, comprising naturally aging the shape cast product for at least 1 day, or at least 2 days, or at least 3 days, or at least 4 days, or at least 5 days, or at least 7 days, or at least 10 days, or at least 15 days, or at least 20 days, or at least 25 days, or at least 30 days, or at least 35 days, or at least 40 days, or at least 45 days.

49. The method of any of claims 39-48, comprising:shipping the shape cast product to a customer, wherein, as shipped, the shape cast product is in an F-temper or a naturally aged temper.

50. The method of any of claims 39-49, comprising:artificially aging the shape cast product, wherein the artificially aging comprises heating the shape cast product to one or more temperatures for a time sufficient to induce precipitation hardening.

51. The method of claim 50, wherein the artificially aging comprises paint baking.

52. The shape cast product of any of the preceding claims, wherein the FeCrMn intermetallic particles comprise a volume fraction of spheroidal FeCrMn intermetallic particles.

53. The shape cast product of claim 52, wherein the volume faction of the spheroidal FeCrMn intermetallic spheroidal intermetallic particles is at least 40 %, or at least 50 %, or at least 60 %, or at least 70 %, or at least 80 %, or at least 90 %.

54. The shape cast product of any of claims 52-53, wherein a majority of the FeCrMn intermetallic particles realize an aspect ratio of not greater than 5: 1, or not greater than 4: 1, or not greater than 3: 1, or not greater than 2.: 1, or not greater than 1.5:1.

55. The shape cast product of any of the preceding claims, wherein the shape cast product realizes an ultimate tensile strength (UTS) of at least 250 MPa, or at least 255 MPa, or at least 260 MPa, or at least 265 MPa, or at least 270 MPa, or at least 275 MPa, or at least 280 MPa, or at least 285 MPa, or at least 290 MPa, or at least 295 MPa, or at least 300 MPa.

56. The shape cast product of any of the preceding claims, wherein the shape cast product realizes a tensile yield strength (TYS) of at least 100 MPa, or at least 105 MPa, or at least 110Attorney Ref. No.: 169593.120026 / WOMPa, or at least 115 MPa, or at least 120 MPa, or at least 125 MPa, or at least 125 MPa, or at least 130 MPa, or at least 135 MPa, or at least 140 MPa.

57. The shape cast product of any of the preceding claims, wherein the shape cast product realizes an elongation of at least 5 %, or at least 6 %, or at least 7 %, or at least 8 %, or at least 9 %, or at least 10 %, or at least 11 %, or at least 12 %, or at least 13 %, or at least 14 %, or at least 15 %.

58. The shape cast product of any of the preceding claims, wherein the shape cast product realizes a quality index of at least 425, or at least 430, or at least 435, or at least 440, or at least 445, or at least 450, or at least 455.

59. The shape cast product of any of the preceding claims, wherein the shape cast product realizes a bend angle of at least 31.5°, or at least 32°, or at least 32.5°, or at least 33°, or at least 33.5°, or at least 34°, or at least 34.5°, or at least 35°, or at least 35.5°, or at least 36°, or at least 36.5°.