Systems and methods for circular manufacturing of mixed metal compounds
Patent Information
- Application Number
- PCT/US2025/032900
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-06-11
- Filing Date
- 2025-06-09
- Publication Date
- 2026-11-19
AI Technical Summary
Existing methods for manufacturing mixed metal compounds generate undesirable by-product gases that are often vented to the atmosphere or discarded as waste due to their chemical nature, environmental impact, and economic loss, with limited recovery and reuse of these gases for producing high-value metal salt precursors.
A method is developed to recover and convert by-product gases into metal salt precursors by absorbing them into specific solutions, such as those containing lithium hydroxide or hydrogen peroxide, followed by oxidation to produce pure compounds like lithium nitrate or lithium sulfate, which are then reused in the production of mixed metal compounds.
This process reduces gas emissions and waste by effectively recycling by-product gases into valuable metal salt precursors, enhancing the production of mixed metal compounds and enabling the extraction of lithium from liquid resources.
Smart Images

Figure US2025032900_19112026_PF_FP_ABST
Abstract
Description
WSGR Docket No. 50741-727.601SYSTEMS AND METHODS FOR CIRCULAR MANUFACTURING OF MIXED METAL COMPOUNDS CROSS-REFERENCE
[0001] This application claims the benefit of U.S. Provisional Application Serial No.63 / 658,831 filed on June 11, 2024, which is hereby incorporated by reference in its entirety.BACKGROUND OF THE INVENTION
[0002] Mixed metal compounds find widespread use across multiple industries, including advanced materials, energy storage, mineral extraction, among others. They include classes of materials oxides or mixed metal oxides, and can include oxides that comprise lithium.
[0003] In some methods, processes, and systems used for the manufacture of mixed metal compounds, a metal salt precursor is mixed with a metal precursor to generate a mixture, and said mixture is heat treated, generating a by-product gas. It may be undesirable to vent said byproduct gas to the atmosphere, due to the chemical nature of said gas, its impact on the environment, discharge permit limits, or simply the economic loss associated with the loss of said gas. Even when by-product gases are removed and recovered through a variety of industrial processes, the absorbed species are typically discarded as waste, in part because the absorbed gas solution contains impurities.
[0004] Herein, methods, processes, and systems are disclosed, which recover said by-product gases and reuse them for conversion into metal salt precursors used in the manufacturing of mixed metal compounds. Said methods, processes, and system include those that absorb the byproduct gases and convert them into precursors, including metal-salt precursors, used in the manufacture of mixed metal compounds.
[0005] In specific aspects described herein, the by-product gases recovered are converted into metal salt precursors and used in the manufacture of a lithium-selective ion exchange material. In a further aspect, said lithium-selective ion exchange material is used to extract lithium from a liquid resource to produce a purified synthetic lithium solution. Lithium is an essential element for high-energy rechargeable batteries and other technologies and can be found in a variety of liquid solutions, including natural and synthetic brines and leachate solutions from minerals and recycled products.SUMMARY OF THE INVENTION
[0006] In one aspect, disclosed herein is a method for preparing a mixed metal compound and reducing gas emissions, the method comprising:WSGR Docket No. 50741-727.601(a) contacting a metal salt precursor with a metal precursor to generate a mixture; (b) heating said mixture to form the mixed metal compound, wherein said heating generates a by-product gas from decomposition of the metal salt precursor, the metal precursor, or any combination thereof;(c) absorbing said by-product gas into an absorber solution to generate an absorbed gas solution; and(d) processing said absorbed gas solution to produce the metal salt precursor, the metal precursor, or any combination thereof.
[0007] In another aspect, disclosed herein is a method for preparing a coated mixed metal compound and reducing gas emissions, the method comprising:(a) contacting a metal salt precursor with a metal precursor to generate a mixture; (b) heating said mixture to form a mixed metal compound and applying a coating to the mixed metal compound to form the coated mixed metal compound, wherein said heating generates a by-product gas from decomposition of the metal salt precursor, a metal precursor, or any combination thereof;(c) absorbing said by-product gases into an absorber solution to generate an absorbed gas solution; and(d) treating said absorbed gas solution to produce the metal salt precursor, the metal precursor, or any combination thereof.
[0008] In yet another aspect, disclosed herein is a method of forming a porous bead, the method comprising:(a) forming a mixed metal compound according to a method for preparing a mixed metal compound and reducing gas emissions as disclosed herein or a coated mixed metal compound according to a method for preparing a coated mixed metal compound and reducing gas emissions as disclosed herein, and(b) combining the mixed metal compound or the coated mixed metal compound with a matrix material,wherein said mixed metal compound or said coated mixed metal compound is embedded in, adhered to, or otherwise supported by the matrix material to form the porous bead.
[0009] In yet another aspect, disclosed herein is a method of extracting lithium from a liquid resource, the method comprising:(a) manufacturing a mixed metal compound according to a method for preparing a mixed metal compound and reducing gas emissions as disclosed herein, a coatedWSGR Docket No. 50741-727.601mixed metal compound according to a method for preparing a coated mixed metal compound and reducing gas emissions as disclosed herein, or a porous bead according to a method for forming a porous bead as disclosed herein, wherein the mixed metal compound, the coated mixed metal compound, or the porous bead selectively exchanges lithium ions and protons;(b) contacting the liquid resource to said mixed metal compound, said coated mixed metal compound, or said porous beads to absorb lithium; and(c) contacting an acidic eluent solution to the mixed metal compound, the coated mixed metal compound, or the porous bead to afford a synthetic lithium solution.
[0010] In yet another aspect, disclosed herein is a mixed metal compound prepared according to a method for preparing a mixed metal compound and reducing gas emissions as disclosed herein, a coated mixed metal compound prepared according to a method for preparing a coated mixed metal compound and reducing gas emissions as disclosed herein, and a porous bead prepared according to a method for forming a porous bead as disclosed herein.
[0011] In yet another aspect, disclosed herein is a method of extracting lithium from a liquid resource, the method comprising:(a) contacting the liquid resource to a mixed metal compound prepared according to a method for preparing a mixed metal compound and reducing gas emissions as disclosed herein, a coated mixed metal compound prepared according to a method for preparing a coated mixed metal compound and reducing gas emissions as disclosed herein, or a porous bead prepared according to a method for forming a porous bead as disclosed hereinto absorb lithium; and(b) contacting an acidic eluent to the mixed metal compound, coated mixed metal compound, or porous bead to afford a synthetic lithium solution.INCORPORATION BY REFERENCE
[0012] All publications, patents, and patent applications mentioned in this specification are herein incorporated by reference to the same extent as if each individual publication, patent, or patent application was specifically and individually indicated to be incorporated by reference.BRIEF DESCRIPTION OF THE DRAWINGS
[0013] The novel features of the disclosure are set forth with particularity in the appended claims. A better understanding of the features and advantages of the present disclosure will be obtained by reference to the following detailed description that sets forth illustrativeWSGR Docket No. 50741-727.601embodiments, in which the principles of the disclosure are utilized, and the accompanying drawings (also “Figure” and “FIG.” herein), of which:
[0014] FIG. 1 provides an overview of the processing steps used in methods for preparing mixed metal compounds, such as those described in Example 1, while concomitantly recovering and regenerating a lithium metal salt precursor used in said methods; this includes a system configured for us in carrying out said method.
[0015] FIGs. 2a-2b provide methods for preparing mixed metal compounds by calcination of a mixture of a metal precursor and a metal salt precursor, such as those described in Example 2a and Example 2b, including a system configured for us in carrying out said method.
[0016] FIGs. 3a-3b provide methods for preparing mixed metal compounds by calcination of a mixture of a metal precursor and a metal salt precursor, such as those described in Example 3a and Example 3b, including a system configured for us in carrying out said method.
[0017] FIG. 4 provides a method for recovering a by-product gas, such as that described in Example 4, including a system configured for use in carrying out said method.
[0018] FIG. 5 provides a method for recovering a by-product gas, such as that described in Example 5, including a system configured for use in carrying out said method.
[0019] FIG. 6 provides a method for recovering a by-product gas, such as that described in Example 6, including a system configured for use in carrying out said method.
[0020] FIG. 7 provides a method for recovering a by-product gas, such as that described in Example 7, including a system configured for use in carrying out said method.
[0021] FIG. 8 provides a method for converting a recovered by-product gas into a metal salt precursor, such as that described in Example 8, including a system configured for use in carrying out said method.
[0022] FIG. 9 provides a method for converting a recovered by-product gas into a metal salt precursor, such as that described in Example 9, including a system configured for use in carrying out said method.
[0023] FIG. 10 provides a method for crystallizing a solid of a metal salt precursor, such as that described in Example 10, including a system configured for use in carrying out said method.
[0024] FIG. 11 provides a method for forming porous beads comprising a mixed metal compound and their use for lithium extraction, such as that described in Example 11, including a system configured for use in carrying out said method.
[0025] FIG. 12 provides a method for forming porous beads comprising a mixed metal compound and their use for lithium extraction, such as that described in Example 12, including a system configured for use in carrying out said method.WSGR Docket No. 50741-727.601
[0026] FIG. 13 provides a method for forming porous beads comprising a mixed metal compound and their use for lithium extraction, such as that described in Example 13, including a system configured for use in carrying out said method.DETAILED DESCRIPTION OF THE INVENTION
[0027] As used herein and in the appended claims, the singular forms “a,” “an,” and “the” include plural referents unless the context clearly dictates otherwise. Thus, for example, reference to “an agent” includes a plurality of such agents, and reference to “the cell” includes reference to one or more cells (or to a plurality of cells) and equivalents thereof known to those skilled in the art, and so forth. When ranges are used herein for physical properties, such as molecular weight, or chemical properties, such as chemical formulae, all combinations and subcombinations of ranges and specific embodiments therein are intended to be included. The term “about” when referring to a number or a numerical range means that the number or numerical range referred to is an approximation within experimental variability (or within statistical experimental error), and thus the number or numerical range, in some instances, will vary between 1% and 15% of the stated number or numerical range. The term “comprising” (and related terms such as “comprise” or “comprises” or “having” or “including”) is not intended to exclude that in other certain embodiments, for example, an embodiment of any composition of matter, composition, method, or process, or the like, described herein, “consist of’ or “consist essentially of’ the described features.
[0028] The terms “lithium”, “lithium ion”, and “Li+” are used interchangeably in the present specification and these terms are synonymous unless specifically noted to the contrary. The terms “hydrogen”, “hydrogen ion”, “proton”, and “H+” are used interchangeably in the present specification and these terms are synonymous unless specifically noted to the contrary.
[0029] As used herein, the words “column” and “vessel” are used interchangeably. In some embodiments described herein referring to a “vessel”, the vessel is a column. In some embodiments described herein referring to a “column”, the column is a vessel.
[0030] The term “the pH of the system” or “the pH of’ a component of a system, for example one or more tanks, vessels, columns, pH modulating units, or pipes used to establish fluid communication between one or more tanks, vessels, columns, or pH modulating units, refers to the pH of the liquid medium contained or present in the system, or contained or present in one or more components thereof. In some embodiments, the liquid medium contained in the system, or one or more components thereof, is a liquid resource. In some embodiments, the liquid mediumWSGR Docket No. 50741-727.601contained in the system, or one or more components thereof, is a brine. In some embodiments, the liquid medium contained in the system, or one or more components thereof, is an acid solution, an aqueous solution, a wash solution, a salt solution, a salt solution comprising lithium ions, or a lithium-enriched solution. As used herein, pH is equal to the negative logarithmic value of the concentration of protons in the aqueous solution. The pH of the solutions described herein are preferably determined with a pH probe. However, many of the solutions described herein comprise high concentrations of ions (e.g., sodium) that are known to interfere with pH probe sensors. Therefore, solutions with high ion concentrations can lead to shifted readings. In such cases, pH probe values are confirmed by diluting the test solution, for example by 10X or 100X, and remeasuring via pH probe to ensure that the change in pH is consistent with the change in concentration of protons. Alternative methods of pH determination include chemical tests such as titration with colored indicators or litmus tests.
[0031] The term “concentration”, as used herein, refers to the amount of a chemical species within a given amount of liquid. In some embodiments, said concentration can be specified as the mass of a species dissolved in an amount of liquid (e.g. mg / L), or the number of moles of a species dissolved in an amount of liquid (e.g. mol / L). In some embodiments, concentration can be specified by the ratio of moles or mass of the species of interest to one or more other species dissolved in the same liquid. In some embodiments, only the mass concentration of an ionic species is stated; for example, a concentration of sodium (Na) is stated to be 100 milligrams per liter (mg / L). In such cases, the stated concentration refers to the mass concentration of the ion in solution, and does not include the mass of the anion; in the example stated above, such an ion may comprise chloride (C1-), nitrate (NO3-), or sulfate (SO42-).
[0032] As used herein, the term “synthetic lithium solution” describes a solution comprising lithium that is not present in nature and obtained by a process for processing, refining, recovering or purifying lithium. In some embodiments, a synthetic lithium solution can be yielded by placing an acid into contact with a lithium-selective sorbent. In some embodiments, a synthetic lithium solution is a lithium eluate. In some embodiments, a synthetic lithium solution is used in place of a liquid resource. In some embodiments, a synthetic lithium solution is combined with a liquid resource. In some embodiments, a synthetic lithium solution is a leachate solution (e.g., a leachate of one or more ores, a leachate of one or more minerals, a leachate of one or more clays, a leachate of waste or recycled materials comprising lithium). In some embodiments, a synthetic lithium solution is a brine concentrated by solar evaporation.WSGR Docket No. 50741-727.601
[0033] The term “direct lithium extraction,” as used herein, refers to a process involving the sorption or adsorption of lithium from solution. Direct lithium extraction can be carried out with a lithium-selective sorbent. A lithium-selective sorbent can comprise an ion exchange material.
[0034] The term “eluate,” as used herein, refers to a liquid input employed for the removal of lithium from a lithium-selective sorbent. An eluate can be acidic. An eluate that has been placed in contact with a lithium-selective sorbent that releases lithium into the eluate is a lithium eluate. A lithium eluate is a synthetic lithium solution. A synthetic lithium solution is a lithium eluate. In some embodiments, wherein the lithium-selective sorbent is an ion exchange material than has been exposed to a liquid resource comprising lithium, the eluate is an acidic solution. In such cases, the protons of the acidic eluate displace the lithium on the ion exchange material to yield a synthetic lithium eluate.
[0035] As used herein, the term “lithium purity” refers to the chemical purity of a lithium chemical, lithium compound, or a solution that comprises lithium or a lithium compound. In some embodiments, lithium purity can be expressed as the percentage of lithium in a solution as on the basis of the total metal ion content of the solution. In some embodiments, lithium purity is expressed in terms of the quantities or percentages of specific impurities that may be present in a lithium compound or a solution that comprises lithium.
[0036] As used herein, the term “process fluid” refers to any liquid or solution that used in any step or process according to the methods and systems for lithium recovery from a liquid resource as described herein. In some embodiments, the process fluid is the liquid resource. In some embodiments, the process fluid is the adjusting fluid. In some embodiments, the process fluid is the raffinate. In some embodiments, the process fluid is water. In some embodiments, the process fluid is acid (e.g., an acidic solution, a solution comprising acid). In some embodiments, the process fluid is base (e.g., a basic solution, a solution comprising base).
[0037] As used herein, the term “buffer” refers to a solution that can resist pH change upon the addition of an acidic or basic components. A buffer can neutralize small amounts of added acid or base, thus maintaining the pH of a solution comprising the buffer. In some embodiments, a buffer is a solution comprising a weak acid and a salt of the corresponding conjugate base. In some embodiments, a buffer is a solution comprising a weak base and a salt of the corresponding conjugate acid. A non-limiting example of a buffer is a solution of boric acid and sodium hydroxide.
[0038] The term “mother liquor,” as used herein, is a liquid byproduct of a process for the generation of solid compound via crystallization from a solution containing the chemical components of said solid compound. In one exemplary embodiment, lithium carbonate isWSGR Docket No. 50741-727.601crystallized from a solution comprising lithium and carbonate ions; the remaining liquid is referred to as a mother liquor, and contains some remaining lithium and carbonate ions, together with additional salts that did not precipitate to form the solid.
[0039] The term “calcination,” as used herein, refers to the thermal treatment of solid chemical compounds, wherein the compound is raised to a high temperature to result in a desirable chemical or physical change. In some embodiments, said change involves a chemical reaction to produce a new chemical compound. In some exemplary embodiments described herein, calcination of a mixture comprising a metal salt precursor and a metal precursor results in the formation of a mixed metal compound. In some embodiments, the one or more chemical compounds in the mixture may melt throughout the calcination treatment. In some embodiments, the one or more chemical compounds in the mixture may remain solid throughout the calcination treatment. In some embodiments, the gaseous atmosphere throughout the calcination process is controlled. In some embodiments, said atmosphere is inert. In some embodiments, the oxygen content in said atmosphere is controlled. In some embodiments, the temperature of the calcination process is constant. In some embodiments, the temperature of the calcination process is higher than 250 °C.
[0040] As used herein, certain chemical species are denoted by a chemical formula which includes x as a subscript. Examples of such species include NOX, SOX, COX. The subscript x indicates that the chemical species comprise one or more possible individual molecules with different possible numbers of oxygen atoms. In some embodiments, x is an integer; in other embodiments, x a fraction or non-integer number. In some embodiments, said individual molecules occur as a mixture. In some embodiments, said individual molecules may interconvert. For example, NOXrefers to either NO (nitric oxide) or NO2(nitrogen dioxide), two common gases, which may interconvert by, for example, the action of light and ozone in the atmosphere. By analogy, SOXrefers to SO, S2O2, SO2, SO3, SO4, S2O (or SO1 / 2), among other chemical species. These chemical species, in some embodiments, include by-product gases generated by the methods and systems described herein.
[0041] As used herein, particle sizes are expressed by a characteristic dimension, where characteristic dimension will be understood to refer to a dimension that reasonably represents the size of a particle to one skilled in the art. For example, said characteristic dimension is typically measured as the diameter for spherical or semi-spherical particles. Particle sizes can be classified by cut off points, typically referred to as a DXX, Dxx, or dxx value, where XX is a number from 1 to 99. XX refers to the percentage of particles that are smaller than the Dxx value, most commonly measured on a volume-weighted basis. For example, a d97 value of 100WSGR Docket No. 50741-727.601microns indicates that 97% of the total particle volume in the sample consists of particles smaller than 100 microns. Similarly, a d10value of 10 microns indicates that 10% of the total particle volume consists of particles smaller than 10 microns. In another usage of the above definition, the parameter D50 specifies that 50% of the particle volume consists of particles larger than the specified value, and 50% of the particle volume consists of particles smaller than the specified value. In some embodiments described herein, the same terminology is applied to the sizes of pores; in such usage, the parameter D50 specifies that 50% of the pore volume is larger than the specified value, and 50% of the pore volume is smaller than the specified value.
[0042] The section headings used herein are for organizational purposes only and are not to be construed as limiting the subject matter described or preclude the combination of the subject matter of the disclosure under any one section heading with any other subject matter of the disclosure under any other section heading or any other subject matter of the disclosure.Embodiments described herein with any one or more features can be readily combined with the features of any embodiments described further herein. Embodiments described herein are not limiting so as to wholly describe all embodiments of the disclosure.General overview of disclosed advances to mixed metal compound preparation
[0043] Mixed metal compounds find widespread use across multiple industries, including advanced materials, energy storage, mineral extraction, among others. In some embodiments, mixed metal compounds include mixed metal oxides. In some embodiments, said mixed metal oxides can comprise one or more metals, wherein one of said metals is lithium.
[0044] In methods, processes, and systems used for the manufacture of mixed metal compound, a metal salt precursor is mixed with a metal precursor to generate a mixture, and said mixture is heat treated, generating a by-product gas. In some methods, processes, and systems, it is undesirable to vent said by-product gas, due to the chemical nature of said has, its impact on the environment, discharge permit limits, or simply the economic loss associated with the loss of said gas.
[0045] Herein, methods, processes, and systems are disclosed, which recover said by-product gases and reuse them for conversion into metal salt precursors used in the manufacturing of mixed metal compounds. In specific aspects described herein, the by-product gases recovered are converted into metal salt precursors and used in the manufacture of a lithium-selective ion exchange material. In a further aspect, said lithium-selective ion exchange material is used to extract lithium from a liquid resource to produce a purified synthetic lithium solution.WSGR Docket No. 50741-727.601
[0046] While by-product gases can be removed and recovered through a variety of industrial processes, the absorbed species are typically discarded as waste, in part because the absorbed gas solution contains impurities.
[0047] In one embodiment of an existing system, for example, a solution of nitric acid and hydrogen peroxide is used to absorb nitrogen oxide by-product gases (NOX) into an aqueous solution to form a more concentrated nitric acid solution. The resulting solution has some value when purified and concentrated for sale or use in separate applications. However, this use does not capture the greater value embodied reusing the nitric acid to produce a high-value metal salt precursor or metal precursor. In another embodiment of an existing system, for example, a solution of NaOH is used to absorb nitrogen oxide by-product gases (NOX) into an aqueous solution, to form a mixture of sodium nitrate and sodium nitrite. However, the resulting solution contains a mixture of nitrate and nitrite salts, which preclude their use for production of mixed metal compounds, which typically require pure compounds. Further, sodium salts are typically inexpensive, rendering it uneconomical to use these salts to produce mixed metal oxide.
[0048] In an aspect of the disclosure described herein, methods and systems are configured to recover the by-product gases in a manner that produces a pure compound, which can be recycled and reused in the production of a mixed metal compound. In one embodiment, the absorbing solution comprises an acidic solution containing the anions of the metal salt precursors, with absorption of the by-product gas providing additional acid and corresponding anions. In another embodiment, the absorbing solution comprises the cation of the metal salt precursor, and the gas is absorbed to provide the anion of the metal salt precursor. In one nonlimiting embodiment, the absorbing solution comprises lithium hydroxide, and the anion is provided by absorbing NOXgases produced by the decomposition of metal salt and metal precursors during the production a mixed metal oxide comprising lithium. In a further nonlimiting embodiment, the absorbing solution comprises oxidizing species that convert a mixture of nitrates and nitrites into a pure solution of nitrate. In a further nonlimiting embodiment, the absorbing solution comprises oxidizing species that ensures oxidation of NOXto into a pure solution of nitrate. In one embodiment, the oxidizing species is hydrogen peroxide. In some embodiments, the mixed metal oxide comprising lithium is a lithium-selective ion exchange material.
[0049] The embodiments described above for the case of nitrogen oxides (NOX) are nonlimiting, and are generally applicable to other volatile oxide by-product gases. In some embodiments, these volatile oxide by-product gases comprise sulfur oxides (SOX). In some embodiments, these volatile oxide by-product gases comprise carbon oxides (COX).WSGR Docket No. 50741-727.601
[0050] For example, a solution of sulfuric acid and hydrogen peroxide can be used to absorb sulfur oxide by-product gases (SOX) into an aqueous solution to form a more concentrated sulfuric acid solution. The resulting solution has some value when purified and concentrated for sale or use in separate applications. However, this use does not capture the greater value embodied reusing the sulfuric acid to produce a high-value metal salt precursor or metal precursor. In another embodiment of an existing system, for example, a solution of NaOH is used to absorb sulfur oxide by-product gases (SOX) into an aqueous solution, to form a mixture of sodium sulfite and sodium sulfate. However, the resulting solution contains a mixture of sulfite and sulfate salts, which preclude their use for production of mixed metal compounds, which typically require pure compounds. In aspects of the disclosure described herein, methods and systems are configured to recover the by-product gases in a manner that produces a pure compound, which can be recycled and reused in the production of a mixed metal compound. In one nonlimiting embodiment, the absorbing solution comprises lithium hydroxide, and the anion is provided by absorbing SOXgases produced by the decomposition of metal salt and metal precursors during the production a mixed metal oxide. In a further nonlimiting embodiment, the absorbing solution comprises oxidizing species that convert a mixture of sulfates and sulfites into a pure solution of sulfate. In a further nonlimiting embodiment, the absorbing solution comprises oxidizing species that ensures oxidation of SOXto into a pure solution of sulfate (SO42’). In one embodiment, the oxidizing species is hydrogen peroxide. In some embodiments, the mixed metal oxide comprising lithium is a lithium-selective ion exchange material.
[0051] In the sections and example that follows, general embodiments of the present disclosure for the production of mixed metal oxide are disclosed.Methods and systems for preparing a mixed metal compound
[0052] An aspect of the present disclosure are systems and methods for preparing a mixed metal compound. Exemplarily embodiments of the present disclosure are given in Examples 1 to 13.
[0053] An aspect of the disclosure described herein is the preparation of a mixed metal compound, said preparation comprising systems and methods wherein the following steps are performed.(1) Contacting a metal salt precursor with a metal precursor to generate a mixture.(2) A heat treatment step in which a mixed metal compound and a by-product gas is produced. In some embodiments, this heat treatment step comprises a calcination process. Examples are given in Examples la, 2a, 2b, 3a, and 3b.WSGR Docket No. 50741-727.601(3) A by-product gas recovery step in which by-product gases are reacted and absorbed into liquid solutions. Some embodiments of this step are described in Examples lb, 4, 5, 6, and 7.(4) Treating said absorbed gas solution to produce a metal salt precursor, a metal precursor, or any combination thereof. Some embodiments of this step include oxidizing converted and absorbed anions to produce a target anion, such as in Examples 1c and 5. Some embodiments comprise conversion of the absorbed gas solution to a lithium salt solution through addition of a carbonate, a hydroxide, or combinations thereof, such as in Examples Id, 8 and 9. Some embodiments include crystallization of said salt into a metal salt precursor for reuse, such as in Examples le, 10, and 11.
[0054] In embodiments of the present disclosure, the above steps can be integrated into a single system or performed as independent unit operations.
[0055] In some embodiments, the metal salt precursor comprises lithium sulfate, the metal precursor comprises titanium dioxide, SOXgases are produced as a by-product of the mixed metal compound Li4Ti5O12product calcination step, SOXgases are optionally oxidized in the gas phase prior to absorption, SOXgases are absorbed with a liquid absorber solution comprising H2O2, sulfuric acid, or combinations thereof the absorber solution is converted to a lithium sulfate solution, and lithium sulfate is crystallized for reuse in the production of the Li4Ti5O12mixed metal compound, such as in Examples 2b, 6, 7, 9, and 11.
[0056] In some embodiments, the metal salt precursor comprises lithium nitrate, the metal precursor comprises titanium dioxide, NOXgases are produced as a by-product of the mixed metal compound Li4Ti5O12product calcination step, NOXgases are absorbed with a liquid absorber solution containing H2O2, NOXgases are optionally absorbed with a liquid absorber solution containing lithium hydroxide with a subsequent oxidation treatment, the absorber solution is converted to a lithium nitrate solution, and lithium nitrate is crystallized for reuse in the production of the Li4Ti5O12mixed metal compound, such as in Examples 2a, 4, 5, 8, and 10.
[0057] In some embodiments, the metal salt precursor comprises lithium nitrate, the metal precursor comprises manganese dioxide, NOXgases are produced as a by-product of the mixed metal compound Li4Mn5O12product calcination step, NOXgases are absorbed with a liquid absorber solution containing H2O2, NOXgases are optionally absorbed with a liquid absorber solution containing lithium hydroxide with a subsequent oxidation treatment, the absorber solution is converted to a lithium nitrate solution, and lithium nitrate is crystallized for reuse in the production of the Li4Mn5O12mixed metal compound, such as in Examples 3a, 4, 5, 8, andWSGR Docket No. 50741-727.601
[0058] In some embodiments, the metal salt precursor comprises lithium sulfate, the metal precursor comprises manganese dioxide, SOXgases are produced as a by-product of the mixed metal compound Li4Mn5O12product calcination step, SOXgases are optionally oxidized in the gas phase prior to absorption, SOXgases are absorbed with a liquid absorber solution comprising H2O2, sulfuric acid, or combinations thereof the absorber solution is converted to a lithium sulfate solution, and lithium sulfate is crystallized for reuse in the production of the Li4Mn5O12mixed metal compound, such as in Examples 3b, 6, 7, 9, and 11.
[0059] In some embodiments, the produced mixed metal compound comprises LiFePO4, LiMnPO4, Li2TiO3, Li2MnO3, Li2SnO3, Li4Ti5O12, Li4Mn5O12, LiMn2O4, Li1.6Mn1.6O4, LiAlO2, LiCuO2, LiTiO2, Li4TiO4, Li7Ti11O24, Li3VO4, Li2Si3O7, Li2CuP2O7, LiNixMnyCo1-x-yO2, LiNixMnyAl1-x-yO2, modifications thereof, solid solutions thereof, or a combination thereof. In some embodiments, the produced mixed metal compound comprises Li2TiO3, Li2MnO3, Li4Ti5O12, Li4Mn5O12, LiMn2O4, Li1.6Mn1.6O4, LiTiO2, Li4TiO4, Li7Ti11O24, modifications thereof, solid solutions thereof, or a combination thereof. In some embodiments, the mixed metal compound comprises Li4Ti5O12or Li4Mn5O12. In some embodiments, the mixed metal compound comprises Li4Ti5O12. In some embodiments, the mixed metal compound comprises Li4Mn5O12.
[0060] In some embodiments, the mixed metal compound is a lithium-selective sorbent. In some embodiments, the mixed metal compound is an ion exchange material, which reversibly exchanges lithium and hydrogen ions. In some embodiments, the mixed metal compound is utilized as the active sorbent in a lithium-selective sorbent composite. In some embodiments, the mixed metal compound is utilized as the active sorbent in a lithium-selective porous bead, such as in Examples 12 and 13. In some embodiments, the mixed metal compound is utilized as a lithium-selective sorbent in a system for extracting lithium from a liquid resource, such as in Examples 12 and 13.
[0061] In some embodiments, the produced mixed metal compound comprises a sodium transition metal oxide. In some embodiments, the produced mixed metal compound comprises a mixed metal compound containing sodium. In some embodiments the mixed metal compound comprises NaFePO4, NaMnPO4, Na2TiO3, Na2MnO3, Na2SnO3, Na4Ti5O12, Na4Mn5O12, NaMn2O4, Na1.6Mn1.6O4, NaA102, NaCuO2, NaTiO2, Na4TiO4, Na7Ti11O24, Na3VO4, Na2Si3O7, Na2CuP2O7, NaNixMnyCo1-x-yO2, or NaNixMnyAl1-x-yO2. In some embodiments the mixed metal compound comprises Na2TiO3, Na2MnO3, Na4Ti5O12, Na4Mn5O12, NaMn2O4, Na1.6Mn1.6O4, NaTiO2, Na4TiO4, or Na7Ti11O24.WSGR Docket No. 50741-727.601
[0062] In some embodiments, the mixed metal compound may be used in energy storage applications as a cathode or anode material. In some embodiments, the mixed metal compound may be used in lithium-ion batteries as a cathode or anode active material. In some embodiments, the mixed metal compound may be used in sodium-ion batteries as a cathode or anode active material.Mixtures of a metal salt precursor with a metal precursor
[0063] In an aspect of the disclosure, a metal salt precursor, a metal precursor, or combinations thereof may be selected for optimized production of a mixed metal compound. In some embodiments, the specific precursor may be selected for its low cost, its melting temperature, its supply chain availability, its production as an intermediate in separate processes, the materials performance characteristics it enables in the product mixed metal compound, or combinations thereof. For example, lithium nitrate has a low melting point temperature and readily forms a molten salt flux when used as a precursor in calcination processes to produce mixed metal compounds. Conversely, lithium sulfate is a common intermediate in lithium-ion battery hydrometallurgical recycling processes, clay and hard rock lithium leach mining processes, and direct lithium extraction processes.
[0064] In an aspect of the disclosure, a metal salt precursor is contacted with a metal precursor to generate a mixture. In some embodiments, the metal salt precursor comprises lithium nitrate, lithium sulfate, lithium carbonate, lithium hydroxide, lithium phosphate, sodium nitrate, sodium sulfate, sodium carbonate, sodium hydroxide, sodium phosphate, lithium nitrite, lithium sulfite, sodium nitrite, sodium sulfite, modifications thereof, solid solutions thereof, or combinations thereof. In some embodiments, the metal salt precursor comprises lithium nitrate, lithium sulfate, or lithium carbonate. In some embodiments, the metal salt precursor comprises lithium nitrate. In some embodiments, the metal salt precursor comprises lithium sulfate. In some embodiments, the metal salt precursor comprises lithium carbonate.
[0065] In some embodiments, the metal salt precursor comprises cations and anions. In some embodiments, the cations comprise lithium, sodium, or combinations thereof. In some embodiments, the anions comprise nitrate, sulfate, carbonate, hydroxide, phosphate, nitrite, sulfite, or combinations thereof.
[0066] In some embodiments, the metal precursor comprises titanium dioxide, titanium alkoxides, manganese dioxide, manganese oxide, manganese carbonate, manganese acetate, manganese hydroxide, tin oxide, tin acetate, tin sulfate, copper oxide, aluminum oxide, vanadium oxide, silicon dioxide, manganese nitrate, manganese sulfate, manganese phosphate,WSGR Docket No. 50741-727.601iron phosphate, ferric nitrate, ferric sulfate, ferrous nitrate, ferrous sulfate, iron oxide, cobalt oxide, NixMnyCo1-x-y(OH)2, NixMnyAl1-x-y(OH)2, solid solutions thereof, or combinations thereof. In some embodiments, the metal precursor comprises titanium dioxide, titanium alkoxides, manganese dioxide, manganese oxide, manganese carbonate, manganese acetate, manganese hydroxide, manganese nitrate, manganese sulfate, manganese phosphate, solid solutions thereof, or combinations thereof. In some embodiments, the metal precursor comprises titanium dioxide, titanium alkoxides, or combinations thereof. In some embodiments, the metal precursor comprises manganese dioxide, manganese oxide, manganese carbonate, manganese acetate, manganese hydroxide, manganese nitrate, manganese sulfate, manganese phosphate, or combinations thereof. In some embodiments, the metal precursor comprises manganese dioxide. In some embodiments, the metal precursor comprises manganese carbonate. In some embodiments, the metal precursor comprises manganese sulfate. In some embodiments, the metal precursor comprises manganese nitrate.
[0067] In some embodiments, the metal salt precursor is lithium nitrate and the metal precursor is titanium dioxide. In some embodiments, the metal salt precursor is lithium sulfate and the metal precursor is titanium dioxide.
[0068] In some embodiments, the metal salt precursor is lithium nitrate and the metal precursor is manganese hydroxide. In some embodiments, the metal salt precursor is lithium sulfate and the metal precursor is manganese hydroxide.
[0069] In some embodiments, the metal salt precursor is lithium nitrate and the metal precursor is manganese carbonate. In some embodiments, the metal salt precursor is lithium sulfate and the metal precursor is manganese carbonate. In some embodiments, the metal salt precursor is lithium nitrate and the metal precursor is manganese dioxide.
[0070] In some embodiments, the metal salt precursor is lithium sulfate and the metal precursor is manganese dioxide. In some embodiments, the metal salt precursor is lithium nitrate and the metal precursor is manganese nitrate. In some embodiments, the metal salt precursor is lithium carbonate and the metal precursor is manganese nitrate.
[0071] In some embodiments, the metal salt precursor is lithium hydroxide and the metal precursor is manganese nitrate. In some embodiments, the metal salt precursor is lithium sulfate and the metal precursor is manganese sulfate. In some embodiments, the metal salt precursor is lithium carbonate and the metal precursor is manganese sulfate. In some embodiments, the metal salt precursor is lithium hydroxide and the metal precursor is manganese sulfate. In some embodiments, the metal salt precursor is lithium hydroxide and the metal precursor is manganese carbonate.WSGR Docket No. 50741-727.601
[0072] In some embodiments, the metal salt precursor is lithium nitrate and the metal precursor is tin oxide. In some embodiments, the metal salt precursor is lithium sulfate and the metal precursor is tin oxide.
[0073] In some embodiments, the metal salt precursor is lithium nitrate and the metal precursor is copper oxide. In some embodiments, the metal salt precursor is lithium sulfate and the metal precursor is copper oxide.
[0074] In some embodiments, the metal salt precursor is lithium nitrate and the metal precursor is manganese phosphate. In some embodiments, the metal salt precursor is lithium sulfate and the metal precursor is manganese phosphate. In some embodiments, the metal salt precursor is lithium phosphate and the metal precursor is manganese nitrate. In some embodiments, the metal salt precursor is lithium phosphate and the metal precursor is manganese sulfate.
[0075] In some embodiments, the metal salt precursor is lithium nitrate and the metal precursor is iron phosphate. In some embodiments, the metal salt precursor is lithium sulfate and the metal precursor is iron phosphate. In some embodiments, the metal salt is lithium phosphate and the metal precursor is ferrous nitrate. In some embodiments, the metal salt is lithium phosphate and the metal precursor is ferrous sulfate.
[0076] In some embodiments, the metal salt precursor is lithium nitrate and the metal precursor is a mixture of iron phosphate and manganese phosphate. In some embodiments, the metal salt precursor is lithium sulfate and the metal precursor is a mixture of iron phosphate and manganese phosphate. In some embodiments, the metal salt is lithium phosphate and the metal precursor is a mixture of ferrous nitrate and manganese nitrate. In some embodiments, the metal salt is lithium phosphate and the metal precursor is a mixture of ferrous sulfate and manganese sulfate.
[0077] In some embodiments, the metal salt precursor is lithium nitrate and the metal precursor is NixMnyCo1-x-y(OH)2, where x is about 0.33 and y is about 0.33, where x is about 0.66 and y is about 0.17, or where x is about 0.8 and y is about 0.1. In some embodiments, the metal salt precursor is lithium sulfate and the metal precursor is NixMnyCo1-x-y(OH)2, where x is about 0.33 and y is about 0.33, where x is about 0.66 and y is about 0.17, or where x is about 0.8 and y is about 0.1.
[0078] In some embodiments, the metal salt precursor is lithium nitrate and the metal precursor is NixCoyAl1-x-y(OH)2, where x is about 0.8 and y is about 0.05, or where x is about 0.84 and y is about 0.12. In some embodiments, the metal salt precursor is lithium sulfate and the metal precursor is NixCoyAl1-x-y(OH)2, where x is about 0.8 and y is about 0.05, or where x is about 0.84 and y is about 0.12.WSGR Docket No. 50741-727.601
[0079] Cationic molar ratio as described here refers to the molar ratio of cations contributed by the metal salt precursor to the cations contributed by the metal precursor. For example, a mixture of lithium nitrate (LiNO3) and titanium dioxide (TiO2) with a cationic ratio of 1: 1 would have 1 mole of lithium nitrate for every mole of TiO2. Conversely, mixture of lithium sulfate (Li2SO4) and titanium dioxide (TiO2) with a cationic ratio of 1: 1 would have 0.5 moles of lithium nitrate for every mole of TiO2. A mixture of metal salt precursor lithium sulfate (Li2SO4) and 1:1 manganese phosphate / iron phosphate would have 1 mole of lithium sulfate, 1 mole of manganese phosphate and 1 mole of iron phosphate.
[0080] In some embodiments, the cationic molar ratio of metal salt precursor to metal precursor is from about 0.7:1 to about 0.8:1. In some embodiments, the cationic molar ratio of metal salt precursor to metal precursor is from about 0.8:1 to about 0.9:1. In some embodiments, the cationic molar ratio of metal salt precursor to metal precursor is from about 0.9: 1 to about 1:1. In some embodiments, the cationic molar ratio of metal salt precursor to metal precursor is from about 1: 1 to about 1:1.5. In some embodiments, the cationic molar ratio of metal salt precursor to metal precursor is from about 2: 1 to about 1:1. In some embodiments, the cationic molar ratio of metal salt precursor to metal precursor is from about 3: 1 to about 2: 1. In some embodiments, the cationic molar ratio of metal salt precursor to metal precursor is from about 4: 1 to about 3:1.
[0081] In some embodiments, the mixture is mixed with a ribbon blender, a v-blender, a vertical cone screw blender, a tumble blender, or combinations thereof. In some embodiments, the mixture is milled together in a ball mill, an attrition mill, a jet mill, or combinations thereof. In some embodiments, the mixture is mixed and stored under inert atmosphere, dry atmosphere, elevated temperatures, or combinations thereof.Heating of mixtures to from a mixed metal compound
[0082] In an aspect of the disclosure, said heating of a mixture of one or more metal salt precursor(s) and one or more metal precursor(s) generates a by-product gas. In some embodiments, said by-product gas is generated by the decomposition of one or more metal salt precursor(s), one or more metal precursor(s), or any combination thereof. In some embodiments, simultaneous to the decomposition of one or all of the precursors is a reaction that forms the target product mixed metal compound.
[0083] In some embodiments, said by-product gas is generated by the decomposition of one or more chemicals that are added to the mixture to facilitate the reaction between the one or more metal salt precursor(s) and the one or more metal precursor(s). In some embodiments, said byproduct gas is generated by the decomposition of one or more liquid(s) that are added to theWSGR Docket No. 50741-727.601mixture to facilitate the reaction between the one or more metal salt precursor(s) and the one or more metal precursor(s). In some embodiments, simultaneous to the decomposition of one or all of the precursors, chemicals, and / or liquids, is a reaction that forms the target product mixed metal compound. Simultaneous to the decomposition of one or all of the precursors is a reaction that forms the target product mixed metal compound.
[0084] In some embodiments, the by-product gas comprises NOX, SOX, CO2, H2O, O2, or combinations thereof. In some embodiments, the by-product gas comprises NOXwherein the metal salt precursor, metal precursor, or combinations thereof contain nitrates. In some embodiments, the by-product gas comprises NOXwherein the metal salt precursor comprises lithium nitrate and releases the by-product gas upon decomposition. In some embodiments, the by-product gas comprises NOXwherein the metal precursor comprises manganese nitrate and releases the by-product gas upon decomposition. In some embodiments, the by-product gas comprises NOXwherein the metal precursor comprises ferrous nitrate and releases the byproduct gas upon decomposition. In some embodiments, the by-product gas comprises SOXwherein the metal salt precursor, metal precursor, or combinations thereof contain sulfates. In some embodiments, the by-product gas comprises SOXwherein the metal salt precursor comprises lithium sulfate and releases the by-product gas upon decomposition. In some embodiments, the by-product gas comprises SOXwherein the metal precursor comprises manganese sulfate and releases the by-product gas upon decomposition. In some embodiments, the by-product gas comprises SOXwherein the metal precursor comprises ferrous sulfate and releases the by-product gas upon decomposition. In some embodiments, the by-product gas comprises COXwherein the metal salt precursor, metal precursor, or combinations thereof contain carbonates. In some embodiments, the by-product gas comprises COXwherein the metal salt precursor comprises lithium carbonate and releases the by-product gas upon decomposition. In some embodiments, the by-product gas comprises COXwherein the metal precursor comprises manganese carbonate and releases the by-product gas upon decomposition. In some embodiments, the by-product gas comprises COXwherein the metal precursor comprises ferrous carbonate and releases the by-product gas upon decomposition.
[0085] In some embodiments, the mixture is heated to a temperature of about 250 to 500 °C. In some embodiments, the mixture is heated to a temperature of about 500 to 750 °C. In some embodiments, the mixture is heated to a temperature of about 750 to 1000 °C. In some embodiments, the mixture is heated to a temperature of about 400 to 950 °C. In some embodiments, the mixture is heated to a temperature of about 250 to 350 °C, 350 to 450 °C, 450 to 550 °C, 550 to 650 °C, 650 to 750 °C, 750 to 850 °C, 850 to 950 °C, or 950 to 1050 °C.WSGR Docket No. 50741-727.601
[0086] In some embodiments the mixture is heated in two stages at different temperatures. In some embodiments, the first stage of the heating occurs at a temperature between 200 and 300 °C and the second stage of the heating occurs at a temperature between 400 and 500 °C. In some embodiments, the first stage of the heating occurs at a temperature between 250 and 500 °C and the second stage of the heating occurs at a temperature between 600 and 800 °C. In some embodiments, the first stage of the heating occurs at a temperature between 250 and 500 °C and the second stage of the heating occurs at a temperature between 800 and 1000 °C. In some embodiments, the first stage of heating occurs at a temperature of about 200 to 250 °C, 250 to 300 °C, 300 to 350 °C, 350 to 400 °C, 400 to 450 °C, or 450 to 500 °C, and the second stage of heating occurs at a temperature of about 500 to 550 °C, 550 to 600 °C, 600 to 650 °C, 650 to 700 °C, 700 to 750 °C, 750 to 800 °C, 800 to 850 °C, 850 to 900 °C, 900 to 950 °C, or 950 to 1000 °C.
[0087] In some embodiments, heating at a lower temperature as a first stage allows for partial reaction and intercalation of the cation from the metal salt precursor into the metal precursor. In some embodiments heating at a lower temperature as a first stage allows for formation of a liquid molten salt flux from melted metal salt precursor, enabling a more uniform reaction of the mixture. In some embodiments, heating to a higher temperature as a second stage allows for more complete reaction of the precursors and crystallization of the correct mixed metal compound phase. In some embodiments, heating to a higher temperature as a second stage creates mixed metal compound with larger crystallites that provide more durability in electrochemical and ion-exchange applications.
[0088] In some embodiments, the temperature and time to which the mixture is heated, either in one or two stages, is adjusted to control the release the by-product gas. In some embodiments, the temperature and time to which the mixture is heated, either in one or two stages, is adjusted to maximize the release the by-product gas. In some embodiments, the temperature and time to which the mixture is heated, either in one or two stages, is adjusted to minimize the release the by-product gas.
[0089] In some embodiments, heating to temperatures ranging from 200 to 300 °C allows for a flux to be formed without significant release of by-product gases. In some embodiments, heating to temperatures ranging from 300 to 400 °C allows for a flux to be formed without significant release of by-product gases. In some embodiments, heating to temperatures ranging from 400 to 500 °C allows for a flux to be formed without significant release of by-product gases.
[0090] In some embodiments, the first stage of heating produces the majority of the by-product gas, with the second stage of heating releasing a minority of the by-product gas. In someWSGR Docket No. 50741-727.601embodiments, the first stage of heating produces the minority of the by-product gas, with the second stage of heating releasing a majority of the by-product gas.
[0091] In some embodiments, the temperature of the heating process may temporarily exceed the target setpoint due to equipment design, thermal gradients within the heating vessel, thermal gradients within the furnace or kiln, limitations in process control algorithms, or combinations thereof. In some embodiments, the maximum allowed temperature of the heating process is limited to a specific upper threshold to prevent formation of undesired crystal phases in the mixed metal compound. In some embodiments, the maximum allowed temperature is about 400 °C. In some embodiments, the maximum allowed temperature is about 450 °C. In some embodiments, the maximum allowed temperature is about 500 °C. In some embodiments, the maximum allowed temperature is about 550 °C. In some embodiments, the maximum allowed temperature is about 600 °C. In some embodiments, the maximum allowed temperature is about 650 °C. In some embodiments, the maximum allowed temperature is about 700 °C. In some embodiments, the maximum allowed temperature is about 750 °C. In some embodiments, the maximum allowed temperature is about 800 °C. In some embodiments, the maximum allowed temperature is about 850 °C. In some embodiments, the maximum allowed temperature is about 900 °C.
[0092] In some embodiments, the heating step duration ranges from about 6 to 12 hours. In some embodiments, the heating step duration ranges from about 12 to 18 hours. In some embodiments, the heating step duration ranges from about 18 to 24 hours. In some embodiments, the heating step duration ranges from about 6 to 8 hours, 8 to 10 hours, 10 to 12 hours, 12 to 14 hours, 14 to 16 hours, 16 to 18 hours, 18 to 20 hours, 20 to 22 hours, or 22 to 24 hours.
[0093] In some embodiments, the temperature ramp rate of the heating step is controlled to about 1 to 2 °C per minute. In some embodiments, the temperature ramp rate of the heating step is controlled to about 2 to 3 °C per minute. In some embodiments, the temperature ramp rate of the heating step is controlled to about 3 to 4 °C per minute. In some embodiments, the temperature ramp rate of the heating step is controlled to about 4 to 5 °C per minute. In some embodiments, the temperature ramp rate of the heating step is controlled to about 5 to 6 °C per minute. In some embodiments, the temperature ramp rate of the heating step is controlled to about 0.5 to 1 °C per minute, 1 to 1.5 °C per minute, 1.5 to 2 °C per minute, 2 to 2.5 °C per minute, 2.5 to 3 °C per minute, 3 to 3.5 °C per minute, 3.5 to 4 °C per minute, 4 to 4.5 °C per minute, 4.5 to 5 °C per minute, 5 to 5.5 °C per minute, or 5.5 to 6 °C per minute.WSGR Docket No. 50741-727.601
[0094] In some embodiments, heating occurs within a pusher kiln, a roller hearth kiln, a rotary kiln, a rotary furnace, a muffle furnace, a batch furnace, or a continuous furnace. In some embodiments, heating is conducted using electrical power to minimize contamination by combustion fuel by-products. In some embodiments, heating is conducted via radiative heating, convective heating, microwave heating, or combinations thereof. In some embodiments heating is conducted by indirectly-fired furnaces or kilns to minimize contamination by combustion byproducts. In some embodiments, heating is conducted by directly-fired furnaces or kilns. In some embodiments, direct-firing utilizes fuels comprising natural gas, propane, syngas, carbon monoxide, hydrogen, or combinations thereof. In some embodiments, direct-firing operates in a fuel-rich or fuel-lean regime to control oxidation state of the product mixed metal compound.
[0095] In some embodiments, the heating step occurs in an indirect-heated rotary calciner. In some embodiments, the indirect-heated rotary calciner is a batch or continuous calciner. In some embodiments, the indirect-heated rotary calciner is configured to operate in batch mode. In some embodiments, the indirect-heated rotary calciner is configured to operate in continuous mode. In some embodiments, the indirect-heated rotary calciner comprises a countercurrent flow of dehumidified air. A countercurrent flow of dehumidified air, according to some embodiments, can reduce the impact of humidity on sintering within the mixed metal compound product during heating. In some embodiments, the indirect-heated rotary calciner comprises a countercurrent flow of low-pressure steam. In some embodiments, the indirect-heated rotary calciner comprises lifter internals. In some embodiments, heating the mixture of metal salt precursor and metal precursor occurs on heated vibrating conveyors.
[0096] In some embodiments, the loaded bed height of the ceramic saggars used to contain the mixture of precursors during the heating step is controlled to maximize uniformity of the reaction, increase uniformity of the mixed metal compound stoichiometry, allow by-product gas release, reduce amount of residual unreacted precursors, or combinations thereof. In some embodiments, the loaded bed height of the mixture of precursors in the ceramic saggars is limited to about 2 to 5 cm. In some embodiments, the loaded bed height of the mixture of precursors in the ceramic saggars is limited to about 5 to 10 cm. In some embodiments, the loaded bed height of the mixture of precursors in the ceramic saggars is limited to about 10 to 15 cm. In some embodiments, the loaded bed height of the mixture of precursors in the ceramic saggars is limited to about 1 to 2 cm, 2 to 4 cm, 4 to 6 cm, 6 to 8 cm, 8 to 10 cm, 10 to 12 cm, or 12 to 15 cm.
[0097] In some embodiments, a rotary kiln or furnace is used to mix precursors more uniformly during the heating process. In some embodiments, knockers are used on the rotary kiln orWSGR Docket No. 50741-727.601furnace during the heating process to reduce build-up of static solid materials within the heating vessel. In some embodiments, rotation speed of the rotary kiln is controlled to optimize mixing of the precursors, reaction rate, dust generation, or combinations thereof. In some embodiments, milling media is added to the mixture of precursors during the heating step in a rotary kiln or furnace to encourage more uniform mixing and reaction. In some embodiments, milling media is utilized during the heating step in a rotary kiln or furnace to reduce the size of the mixed metal compound product within the same unit operation.
[0098] In some embodiments, heating occurs within a controlled gas atmosphere supplied by fresh gas comprising air, oxygen, nitrogen, or combinations thereof. In some embodiments, the level of oxygen in the supply of fresh gas is controlled to maintain the correct oxidation state of the cations in the mixed metal compound. In some embodiments, the supply of fresh gas has oxygen levels ranging from about 0 to 20 volume percent. In some embodiments, the supply of fresh gas has oxygen levels ranging from about 20 to 40 volume percent. In some embodiments, the supply of fresh gas has oxygen levels ranging from about 40 to 60 volume percent. In some embodiments, the supply of fresh gas has oxygen levels ranging from about 60 to 80 volume percent. In some embodiments, the supply of fresh gas has oxygen levels ranging from about 80 to 100 volume percent. In some embodiments, the supply of fresh gas is controlled to reduce moisture content. In some embodiments, the dew point of the supply of fresh gas is controlled to about -40 to -70 °C. In some embodiments, the dew point of the supply of fresh gas is controlled to about -10 to -40 °C. In some embodiments, the dew point of the supply of fresh gas is controlled to about 0 to -20 °C.
[0099] In some embodiments, the supplied gas into the heating chamber is pre-heated to the target temperature of the mixture of metal salt precursor and metal precursor. In some embodiments, the supplied gas into the heating chamber is directed through antechambers or piping contained within the furnace or kiln to pre-heat the gas. In some embodiments, the supplied gas is fed at ambient external temperatures and allowed to heat up upon entry to the heating chamber.
[0100] In some embodiments, the exchange rate of fresh gas into the controlled atmosphere of the heating step is controlled to control reaction rate, heating rate of the mixture, by-product gas concentration in the controlled atmosphere and exhaust stream, or combinations thereof. In some embodiments, the controlled gas atmosphere of the heating step has a fresh gas exchange rate of about 5 to 50 vessel volumes per hour. In some embodiments, the controlled gas atmosphere of the heating step has a fresh gas exchange rate of about 50 to 100 vessel volumes per hour. In some embodiments, the controlled gas atmosphere of the heating step has a fresh gas exchangeWSGR Docket No. 50741-727.601rate of about 100 to 150 vessel volumes per hour. In some embodiments, the controlled gas atmosphere of the heating step has a fresh gas exchange rate of about 1 to 5 vessel volumes per hour, 5 to 10 vessel volumes per hour, 10 to 20 vessel volumes per hour, 20 to 30 vessel volumes per hour, 30 to 40 vessel volumes per hour, 40 to 50 vessel volumes per hour, 50 to 60 vessel volumes per hour, 60 to 70 vessel volumes per hour, 70 to 80 vessel volumes per hour, 80 to 90 vessel volumes per hour, 90 to 100 vessel volumes per hour, 100 to 110 vessel volumes per hour, 110 to 120 vessel volumes per hour, 120 to 130 vessel volumes per hour, 130 to 140 vessel volumes per hour, or 140 to 150 vessel volumes per hour.Absorption of by-product gases
[0101] In an aspect of the disclosure, by-product gases are converted and absorbed by an absorber liquid to form an absorbed gas solution. This absorption allows for recovery of the byproduct gases for further treatment and conversion to a reagent precursor for reuse in the overall system. Simultaneously, by-product gases may be regulated as air pollutants and may require emissions mitigation systems. Absorption of the by-product gases into an absorber liquid serves the dual function of recovering reagents for reuse and reducing air pollutant emissions.
[0102] In an aspect of the disclosure described herein, methods and systems are configured to recover the by-product gases in a manner that produces a pure compound, which can be recycled and reused in the production of a mixed metal compound. In one embodiment, the absorbing solution comprises the cation of the metal salt precursor, and the gas is absorbed to provide the anion of the metal salt precursor. In one nonlimiting embodiment, the absorbing solution comprises lithium hydroxide, and the anion is provided by absorbing NOXgases produced by the decomposition of metal salt and metal precursors during the production a mixed metal oxide comprising lithium. In a further nonlimiting embodiment, the absorbing solution comprises oxidizing species that convert a mixture of nitrates and nitrites into a pure solution of nitrate. In one embodiment, the oxidizing species is hydrogen peroxide. In some embodiments, the mixed metal oxide comprising lithium is a lithium-selective ion exchange material.
[0103] In some embodiments, the by-product gases are cooled to just about the boiling point of the gas to improve absorption efficiency, reduce heat load on the absorber system, reduce thermal decomposition of oxidants in the absorber system, or combinations thereof, while avoiding condensation of gases in the cooling system. In some embodiments, the by-product gases are cooled to about -5 to 0 °C, 0 to 5 °C, 5 to 10 °C, 10 to 15 °C, 15 to 20 °C, 20 to 25 °C, 25 to 30°C, 30 to 35 °C, 35 to 40 °C, 40 to 45 °C, 45 to 50 °C, 50 to 55 °C, 55 to 60 °C, 60 to 65 °C, 65 to 70 °C, 70 to 75 °C, 75 to 80 °C, 80 to 85 °C, 85 to 90 °C, 90 to 95 °C, or 95 to 100 °C.WSGR Docket No. 50741-727.601In some embodiments, the by-product gases comprise NOXand is cooled to about 25 to 30 °C. In some embodiments, the by-product gases comprise NOXand is cooled to about 30 to 40 °C. In some embodiments, the by-product gases comprise NOXand is cooled to about 40 to 50 °C. In some embodiments, the by-product gases comprise SOXand is cooled to about 5 to 10 °C. In some embodiments, the by-product gases comprise SOXand is cooled to about 10 to 20 °C. In some embodiments, the by-product gases comprise SOXand is cooled to about 20 to 30 °C.
[0104] In some embodiments, the by-product gas is cooled to partially or completely condense the by-product gas into a liquid prior to absorption. In some embodiments, the by-product gases comprise NOX, a mixture of NO and NO2 gases, and NO2 is condensed via passing the byproduct gas through a heat exchanger that cools the gas to below about 21 °C. In some embodiments, this liquid NO2 directly transferred to an absorber liquid system where it is oxidized and converted to nitric acid. In some embodiments, the NO and a portion of the NO2 gas is exhausted to a liquid absorber system for reaction and absorption into an absorbed gas solution.
[0105] In some embodiments, the by-product gases comprise SOX, a mixture of SO, SO2, and SO3 gases, and SO2 and SO3 are condensed via passing the by-product gas through a heat exchanger that cools the gas to below about -10 °C. In some embodiments, SO2 forms the majority of the condensate and is transferred as a liquid to an absorber liquid system where it is oxidized and converted to sulfuric acid. In some embodiments, SO3 solids may form from the cooled by-product gas stream and is periodically purged from the heat exchanger as SO3 gas by heating the heat exchanger to above about 32.5 °C, 45 °C, or 62.3 °C. In some embodiments, the resulting SO3 gas is directly transferred to the liquid absorption system to form an absorbed gas solution comprising sulfuric acid.
[0106] In some embodiments, the by-product gas is oxidized prior to absorption into the absorber solution. In some embodiments, the by-product gas is oxidized by passing the gas over a catalyst in the presence of oxygen, an example of which is shown in Example 6. In some embodiments, the by-product gas is oxidized prior to absorption by mixing the gases with an oxidizing gas comprising chlorine, ozone, oxygen, or combinations thereof. In some embodiments, the by-product gas is oxidized as it reacts and absorbs into the absorber solution, an example of which is shown in Examples 4 and 7. In some embodiments, oxidation occurs after absorption and the anions in the absorber solution are oxidized by mixing the solution with an oxidizer, an example of which is shown in Example 5. In some embodiments, the oxidizer in this step comprises hydrogen peroxide, oxygen, ozone, chlorine, or combinations thereof.WSGR Docket No. 50741-727.601
[0107] In some embodiments, the by-product gas is absorbed onto a solid sorbent. In some embodiments, the solid sorbent comprises lithium hydroxide, lithium carbonate, or combinations thereof. In some embodiments, the solid sorbent is sprayed into an absorber tower as a slurry to absorb the by-product gas. In some embodiments, the solids formed from absorption comprise lithium nitrite, lithium nitrate, lithium sulfite, lithium sulfate, or combinations thereof. In some embodiments, the solids formed from absorption are oxidized in contact with another oxidant comprising air, ozone, hydrogen peroxide, or combinations thereof. In some embodiments, the solids formed from absorption are dissolved into an aqueous solution to allow for further purification and separation into a metal salt precursor. In some embodiments, the solids formed from absorption may be directly used as a metal salt precursor.
[0108] In some embodiments, the by-product gas is absorbed into an absorber solution within a wet absorber system. In some embodiments, the absorber system comprises packed tower absorbers, spray tower absorbers, venturi absorbers, ejection venturi absorbers, tray-type absorbers, cyclone absorbers or combinations thereof. In some embodiments, the packed tower absorbers utilize random packing. In some embodiments, the random packing comprises Raschig rings, pall rings, VSP rings, Dixon rings, Cannon rings, conjugate rings, Cascade mini rings, super Raschig Rings, Intalox saddle rings, HY-pack rings, polyhedral hollow balls, hollow float balls, heilex rings, cross spherical rings, lantern rings, snowflake rings, Hi-Flow rings, TriPack rings, Q-pack rings, pentagon rings, or combinations thereof. In some embodiments, the packed tower absorbers utilize structured packing.
[0109] In some embodiments, the absorption tower includes one or more de-misting components, wherein said components serve to remove any liquid entrained in the gas existing the absorber, such that said gas is substantially free of liquid. In some embodiments, said demister is a demister pad. In some embodiments, said demister is a porous structure. In some embodiments, said demister component is constructed out of a metal, a ceramic, a polymer, or a combination thereof.
[0110] In some embodiments, the absorber system utilizes storage tanks to hold absorber solution that is recirculated within the wet absorbers. In some embodiments, the absorber system utilizes heat exchangers, jacketed tanks, or combinations thereof to maintain a maximum operating temperature for the absorber solution. In some embodiments, the temperature of the absorber is maintained at about under 60 °C. In some embodiments, the temperature of the absorber is maintained at about under 50 °C. In some embodiments, the temperature of the absorber is maintained at about under 40 °C. In some embodiments, the temperature of the absorber is maintained at about under 30 °C. In some embodiments, the temperature of theWSGR Docket No. 50741-727.601absorber is maintained at about under 20 °C. In some embodiments, the temperature of the absorber is maintained at about under 10 °C. In some embodiments, the absorber solution is described as an absorbed gas solution after some absorption of the by-product gas.
[0111] In some embodiments, the absorber system comprises a single absorber. In some embodiments, the absorber system comprises two absorbers in series. In some embodiments, the absorber system comprises three or more absorbers in series. In some embodiments, the absorber system comprises two or more trains of absorbers in parallel for redundancy or increased treatment capacity.
[0112] In some embodiments, the absorber solution comprises an aqueous solution of sulfuric acid, nitric acid, hydrogen peroxide or combinations thereof. In some embodiments, the absorber solution comprises an aqueous solution of sulfuric acid and hydrogen peroxide. In some embodiments, the absorber solution comprises an aqueous solution of nitric acid and hydrogen peroxide. In some embodiments, the hydrogen peroxide concentration in the absorber solution is maintained during absorption at a level of at least 1 wt%. In some embodiments, the hydrogen peroxide concentration in the absorber solution is maintained during absorption at a level of at least 2 wt%. In some embodiments, the hydrogen peroxide concentration in the absorber solution is maintained during absorption at a level of at least 3 wt%. In some embodiments, the hydrogen peroxide concentration in the absorber solution is maintained during absorption at a level of at least 0.5 wt%, 1 wt%, 1.5 wt%, 2 wt%, 2.5 wt%, 3 wt%, 3.5 wt%, 4 wt%, 4.5 wt%, or 5 wt%. In some embodiments, the nitric acid concentration in the absorbed gas solution is maintained during absorption at a level of no more than about 25 wt%. In some embodiments, the nitric acid concentration in the absorbed gas solution is maintained during absorption at a level of no more than about 35 wt%. In some embodiments, the nitric acid concentration in the absorbed gas solution is maintained during absorption at a level of no more than about 45 wt%. In some embodiments, the nitric acid concentration in the absorbed gas solution is maintained during absorption at a range between about 0 and 5 wt%, 5 and 10 wt%, 10 and 15 wt%, 15 and 20 wt%, 20 and 25 wt%, 5 and 25 wt%, 25 and 30 wt%, 30 and 35 wt%, 5 and 35 wt%, 35 and 40 wt%, 40 and 45 wt%, 5 and 45 wt%, 45 and 50 wt%, 50 and 55 wt%, 55 and 60 wt%, or 60 and 65 wt%. In some embodiments, the sulfuric acid concentration in the absorbed gas solution is maintained during absorption at a level of between about 99 to 100 wt%. In some embodiments, the sulfuric acid concentration in the absorbed gas solution is maintained during absorption at a level of at least 97%. In some embodiments, the sulfuric acid concentration in the absorbed gas solution is maintained during absorption at a level of no more than about 10 wt%. In some embodiments, the sulfuric acid concentration in the absorbed gas solution is maintainedWSGR Docket No. 50741-727.601during absorption at a level of no more than about 10 wt%, 20 wt%, 30 wt%, 40 wt%, 50 wt%, 60 wt%, 70 wt%, 80 wt%, 90 wt%, or 97 wt%.
[0113] In some embodiments, the absorber solution comprises an alkaline aqueous solution. In some embodiments, the absorber solution comprises an alkaline aqueous solution of lithium hydroxide. In some embodiments, the concentration of lithium hydroxide in the absorber solution prior to absorption is about 5 wt%, 10 wt%, 15 wt%, 20 wt%, 25 wt%, or 30 wt%. In some embodiments, the alkaline absorber solution comprises lithium nitrite, lithium nitrate, lithium hydroxide, or combinations thereof. In some embodiments, the alkaline absorber solution comprises lithium sulfite, lithium sulfate, lithium hydroxide, or combinations thereof. In some embodiments, an alkaline absorber solution is used for polishing absorption after primary absorption of by-product gas in an acidic absorber solution. In some embodiments, the alkaline absorber solution is used for absorption until alkalinity is neutralized and the pH of the solution reaches about 7. In some embodiments, the alkaline absorber solution pH is maintained at about at least about pH 8. In some embodiments, the alkaline absorber solution pH is maintained at about at least about pH 9. In some embodiments, the alkaline absorber solution pH is maintained at about at least about pH 10. In some embodiments, the alkaline absorber solution pH is maintained at about at least about pH 11. In some embodiments, the alkaline absorber solution pH is maintained at about at least about pH 12. In some embodiments, the alkaline absorber solution pH is maintained at about at least pH 8, 9, 10, 11, 12, 13, or 14. In some embodiments, the alkaline absorber solution is mixed with an oxidizer comprising hydrogen peroxide, oxygen, air, ozone, or combinations thereof to oxidize nitrite anions to nitrate. In some embodiments, the alkaline absorber solution is mixed with an oxidizer comprising hydrogen peroxide, oxygen, air, ozone, or combinations thereof to oxidize sulfite anions to sulfate. In some embodiments, the alkaline absorber solution is mixed with an acidic absorber solution containing an oxidant to oxidize the anions within the alkaline absorber solution feed, an example of which is described in Example 7. In some embodiments, the alkaline absorber solution is mixed with an acidic absorber solution containing hydrogen peroxide oxidize the anions within the alkaline absorber solution feed.
[0114] In some embodiments, the by-product gases comprise NOX, the one or more absorbers contain an alkaline aqueous solution comprising lithium hydroxide, and the oxidizing agent contain one of the said one or more absorbers comprises hydrogen peroxide. In some embodiments, one or more of the following chemical reactions occur in said aqueous solution, wherein all reactions occur should be understood to represent an equilibrium state of chemicalWSGR Docket No. 50741-727.601species. In some embodiments, the ultimate result of the reactions is the production or a metal salt precursor. In some embodiments, said metal salt precursor is lithium nitrate.N2O4(aq)+H2O → HNO2+ HNO3NO2(aq)+H2O → HNO2+ HNO3N2O3(aq)+H2O →2 HNO2LiOH (aq) + HNO2→ LiNO2+ H2OLiOH (aq)+ HNO3 LiNO3+ H2OLiNO2(aq) + H2O2→ LiNO3+ H2OLiOH (aq) + HNO3(aq) → LiNO3(aq) + H2OLiNO2(aq) + 2 HNO3(aq) → 2NO2(g) + LiNO3+H2O2LiNO2(aq) + 2HNO3(aq) → 2LiNO3+ NO2(g) +NO (g) + H2O
[0115] In some embodiments, the by-product gases comprise SOX, the one or more absorbers contain an alkaline aqueous solution comprising lithium hydroxide, and the oxidizing agent contain one of the said one or more absorbers comprises hydrogen peroxide. In some embodiments, one or more of the following chemical reactions occur in said aqueous solution, wherein all reactions occur should be understood to represent an equilibrium state of chemical species. In some embodiments, the ultimate result of the reactions is the production or a metal salt precursor. In some embodiments, said metal salt precursor is lithium sulfate.SO3(aq)+H2O → H2SO4SO2(aq)+H2O → H2SO32 LiOH (aq) + H2SO3→ Li2SO3+ 2 H2O2 LiOH (aq)+ H2SO4→ Li2SO4+ 2 H2OLi2SO3(aq) + H2O2→ Li2SO4+ H2OTreatment of absorbed gas solutions to produce a metal salt precursor or a metal precursor
[0116] In an aspect of this system, the solution produced from absorption of by-product gases by an absorber solution is described as an absorbed gas solution. In some embodiments, the absorbed gas solution is transferred from the absorber system to a separate conversion system for further treatment to produce a metal salt precursor or a metal precursor.
[0117] In some embodiments, lithium carbonate, lithium hydroxide, or combinations thereof are added to the absorbed gas solution to neutralize acids present and convert the solution to a metal salt precursor solution. Herein, the molar ratio (atomic lithium basis) of combinations of lithiumWSGR Docket No. 50741-727.601carbonate (Li2CO3) and lithium hydroxide (LiOH) refers to the ratio of moles of lithium derived from lithium carbonate to the moles of lithium derived from lithium hydroxide. For example, one mole of lithium carbonate mixed with one mole of lithium hydroxide would result in a molar ratio (atomic lithium basis) of lithium carbonate and lithium hydroxide of 2: 1. In some embodiments, the molar ratio (atomic lithium basis) of lithium carbonate to lithium hydroxide added the absorbed gas solution ranges from about 90:10 to 97:3. In some embodiments, the molar ratio (atomic lithium basis) of lithium carbonate to lithium hydroxide added the absorbed gas solution ranges from about 10:90 to 90:10. In some embodiments, the molar ratio (atomic lithium basis) of lithium carbonate to lithium hydroxide added the absorbed gas solution ranges from about 0:100 to 10:90. In some embodiments, the molar ratio (atomic lithium basis) of lithium carbonate to lithium hydroxide added the absorbed gas solution ranges from about 0:100 to 5:95, 5:95 to 10:90, 10:90 to 15:85, 15:85 to 20:80, 20:80 to 25:75, 25:75 to 30:70, 30:70 to 35:65, 35:65 to 40:60, 40:60 to 45:55, 45:55 to 50:50, 50:50 to 55:45, 55:45 to 60:40, 60:40 to 65:35, 65:35 to 70:30, 70:30 to 75:25, 75:25 to 80:20, 80:20 to 85:15, 85:15 to 90:10, 90:10 to 95:5, or 95:5 to 100:0.
[0118] In embodiments where lithium carbonate is added to neutralize acids present, carbon dioxide is produced. In some embodiments, said carbon dioxide bubbles out of the neutralized solution. In some embodiments, it is preferable to maximize usage of lithium carbonate over lithium hydroxide due to lower health hazards, lower reagent cost, increased shelf stability, or combinations thereof. In some embodiments, it is preferable to maximize usage of lithium hydroxide due to simpler reaction dynamics (e.g. no off-gassing, foaming, or pH buffering), reduced formation of dissolved carbonate and bicarbonate species, reduced carbonate scaling, or combinations thereof. In some embodiments, a combination of lithium carbonate and lithium hydroxide is used to take advantage of a mix of the aforementioned advantages. In some embodiments, lithium carbonate is added to the absorbed gas solution until a pH of about 0.5-1 is achieved, and lithium hydroxide is added to further increase the pH of the solution to a final pH of about 7, 8, 9, 10 or 11. In some embodiments, lithium hydroxide is added as an aqueous solution, a solid powder, or combinations thereof.
[0119] In some embodiments, sodium bicarbonate, sodium carbonate, sodium hydroxide, or combinations thereof are added to the absorbed gas solution to neutralize acids present and convert the solution to a metal salt precursor solution. In some embodiments, manganese hydroxide, manganese carbonate, manganese ore, or combinations thereof are added to the absorbed gas solution to neutralize acids present and convert the solution to a metal precursor solution. In some embodiments, ferrous hydroxide, ferrous carbonate, metallic iron, orWSGR Docket No. 50741-727.601combinations thereof are added to the absorbed gas solution to neutralize acids present and convert the solution to a metal precursor solution.
[0120] In some embodiments, the absorbed gas solution may contain undesirable impurities. In some embodiments, the impurities comprise solid particulates, dissolved calcium, dissolved magnesium, dissolved transition metal species, or combinations thereof. In some embodiments, the dissolved transition metal species comprise iron, manganese, titanium, nickel, cobalt, copper, chromium, or combinations thereof. In some embodiments, the undesired impurities are removed with hydrometallurgical processes, filtration, ion-exchange, adsorption, membrane filtration, or combinations thereof. In some embodiments, dissolved impurities are precipitated by increasing the pH of the absorbed gas solution. In some embodiments, this increase in pH is achieved with the addition of lithium carbonate, lithium hydroxide, or combinations thereof. In some embodiments, this increase in pH is achieved with the addition of sodium bicarbonate, sodium carbonate, sodium hydroxide, or combinations thereof. In some embodiments, oxidants are introduced to the absorbed gas solution to oxidize dissolved transition metal species in the solution and facilitate oxidation.
[0121] In some embodiments, the converted absorbed gas solution is filtered to remove residual solids and precipitates prior to further processing. In some embodiments, the absorbed gas solution is filtered to remove residual solids and precipitates prior to further processing. In some embodiments, filtration occurs in a filtration system comprising a bag filter, a candle filter, a cartridge filter, a media filter, a depth filter, a sand filter, a membrane filter, an ultrafiltration system, a microfiltration filter, a nanofiltration filter, a cross-flow filter, a dead-end filter, a drum filter, a filter press, or a combination thereof. In some embodiments, residual solids and precipitates are separated from the converted absorbed gas solution by sedimentation, centrifugation, thickening, flocculation, coagulation, or combinations thereof. In some embodiments, an absorbed gas solution following filtration is termed a filtered absorbed gas solution.
[0122] In some embodiments, nitric acid is added to the converted absorbed gas solution to slightly acidify the solution and reduce presence of dissolved bicarbonate and carbonate species. In some embodiments, nitric acid is added to the absorbed gas solution to slightly acidify the solution and reduce presence of dissolved bicarbonate and carbonate species. In some embodiments, nitric acid is added to the filtered absorbed gas solution to slightly acidify the solution and reduce presence of dissolved bicarbonate and carbonate species. In some embodiments, sulfuric acid is added to the converted absorbed gas solution to slightly acidify the solution and reduce presence of dissolved bicarbonate and carbonate species. In someWSGR Docket No. 50741-727.601embodiments, the pH is lowered to about 7 or less. In some embodiments, the pH is lowered to about 6 or less. In some embodiments, the pH is lowered to about 5 or less. In some embodiments, the pH is lowered to about 3.5 or less. In some embodiments, the pH is lowered to about 7. In some embodiments, the pH is lowered to about 5. In some embodiments, the pH is lowered to about 3.5. In some embodiments, vacuum is pulled on the solution after lowering the pH to facilitate degassing and removal of dissolved CO2.
[0123] In some embodiments, the converted absorbed gas solution is crystallized to produce a slurry containing metal salt precursor or metal precursor solids. In some embodiments, the absorbed gas solution is crystallized to produce a slurry containing metal salt precursor or metal precursor solids. In some embodiments, the filtered absorbed gas solution is crystallized to produce a slurry containing metal salt precursor or metal precursor solids. In some embodiments, the converted absorbed gas solution is concentrated in a concentration system prior to crystallization to facilitate crystallization. In some embodiments, the absorbed gas solution is concentrated in a concentration system prior to crystallization to facilitate crystallization. In some embodiments, the filtered absorbed gas solution is concentrated in a concentration system prior to crystallization to facilitate crystallization. In some embodiments, the converted absorbed gas solution is fed into a continuous crystallization system where the elevated mother liquor concentration is maintained via evaporator systems. In some embodiments, the absorbed gas solution is fed into a continuous crystallization system where the elevated mother liquor concentration is maintained via evaporator systems. In some embodiments, the filtered absorbed gas solution is fed into a continuous crystallization system where the elevated mother liquor concentration is maintained via evaporator systems. In some embodiments, the temperature of the slurry and mother liquor is maintained at a set point to prevent formation of undesired hydrate or anhydrous phases of metal salt precursor or metal precursor.
[0124] In some embodiments, the conversion system comprises a conversion reactor system, a filtration system, a liquid concentration system, a crystallizer system, a solid-liquid separation system, a drying system, or combinations thereof. In some embodiments, the conversion reactor system comprises jacketed continuous stir tank reactors, forced circulation reactors with heat exchangers for thermal management, stir tank reactors with no thermal management, or passively-cooled stir tank reactors. In some embodiments of the conversion system, the treated absorbed gas solution is first treated to remove water in a liquid concentration system, followed by crystallization of a metal salt solution in a crystallization system. In some embodiments of the conversion system, the absorbed gas solution is first treated to remove water in a liquidWSGR Docket No. 50741-727.601concentration system, followed by crystallization of a metal salt solution in a crystallization system. In some embodiments of the conversion system, the filtered absorbed gas solution is first treated to remove water in a liquid concentration system, followed by crystallization of a metal salt solution in a crystallization system. Exemplary embodiments are included in Examples 10 and 11.
[0125] In some embodiments, the liquid concentration system comprises reverse osmosis membrane systems, osmotically-assisted reverse osmosis membrane systems, mechanical vapor recompression evaporators, single-effect evaporators, multiple-effect evaporators, falling film evaporators, natural circulation evaporators, forced circulation evaporators, modifications thereof, or combinations thereof.
[0126] In some embodiments of the liquid concentration system, water is evaporated off the absorbed gas solution, converted absorbed gas solution, or other liquid stream. In some embodiments, said liquid concentration system comprises an evaporator system. In some embodiments, the evaporator operates at a temperature from about zero to about 200 °C. In some embodiments, the evaporator operates at a temperature of about 0 - 10, 10 - 20, 20 - 30, 30 -40, 40 - 50, 50 - 60, 60 -70, 70 - 80, 80 - 90, 90 - 100, 100, 110, 110 - 120, 120 - 130, 130 -150, 150 - 175, or 175 - 200 °C. In a preferred embodiment, the temperature is about 90 °C. In some embodiments, the evaporator operates at a pressure from about 0.1 psia (wherein psi denotes absolute - and not relative - pressure) to 100 psi a. In some embodiments, the evaporator operates at a pressure of about 0.1 - 1, 1 - 2, 2 - 4, 4 - 6, 6 - 10, 10 - 20, 20 - 50, or 50 - 10 psia. In a preferred embodiment, the pressure is about 1 psia. In some embodiments, the final concentration of the metal salt precursor in the liquid existing the liquid concentration system is from 0.1 to 99 weight %. In preferred embodiments, the concentration of the metal salt precursor in the liquid exiting the liquid concentration system is from 60 to 80 weight %. In some embodiments, the final concentration of the metal salt precursor in the liquid exiting the liquid concentration system is from about 0.1 to about 1, from about 1 to about 5, from about 5 to about 10, from about 10 to about 20, from about 20 to about 30, from about 30 to about 40, from about 40 to about 50, from about 50 to about 60, from about 60 to about 70, from about 70 to about 80, from about 80 to about 90, from about 90 to about 99.9 weight %.
[0127] In some embodiments of the conversion system, the liquid exiting the liquid concentration system is sent to crystallization system, where the metal salt solution is crystallized. In some embodiments of the crystallization system, the metal salt precursor or metal precursor solids are separated from the crystallization mother liquor with a solid-liquid separation system. In some embodiments of the crystallization system, the temperature of theWSGR Docket No. 50741-727.601liquid is lowered to crystallize the lithium salt precursor. In some embodiments, the temperature is about 0 - 10, 10 - 20, 20 - 30, 30 - 40, 40 - 50, 50 - 60, 60 -70, 70 - 80, 80 - 90, 90 - 100, 100, 110, 110 - 120, 120 - 130, 130 - 150, 150 - 175, or 175 -200 °C. In a preferred embodiment, the temperature is about 50 °C. In some embodiments, the temperature of the slurry and mother liquor is maintained at a set point to prevent formation of undesired hydrate or anhydrous phases of metal salt precursor or metal precursor.
[0128] In some embodiments, the crystallizer system comprises continuously stirred tank reactors, baffled stirred tank reactors, agitated tank reactors, draft tube baffle crystallizers, forced circulation crystallizers, Oslo crystallizers, classified bed crystallizers, cooling crystallizers, vacuum cooling crystallizers, continuous cooling crystallizers, scraped surface crystallizers, or combinations thereof. In some embodiments, the solid liquid separation system comprises clarifiers, thickeners, centrifuges, pusher centrifuges, peeler centrifuges, basket centrifuges, filter presses, continuous centrifuges, batch centrifuges, or combinations thereof. In some embodiments, the drying system comprises a fluid bed dryer, a vacuum tray dryer, a forced circulation tray dryer, a vacuum belt dryer, a vacuum rotary dryer, a hollow flight screw conveyor dryer, or combinations thereof.
[0129] In some embodiments, the separated solids are transferred to a drying system to form dry metal salt precursor or metal precursor. In some embodiments, the drying system is maintained at a temperature of at least about 30 °C, 40 °C, 50 °C, 60 °C, 70 °C, 80 °C, 90 °C, 100 °C, 110 °C, 120 °C, 130 °C, 140 °C, 150 °C, 160 °C, 170 °C, 180 °C, 190 °C, 200 °C, 210 °C, 220 °C, 230 °C, 240 °C, or 250 °C.
[0130] Exemplary embodiments describing the treatment of an absorbed gas solution to produce a metal salt precursor or metal precursor are described in Examples 4 to 10.Reduction of gas emissions
[0131] An aspect of the disclosure is the reduction of by-product gas emissions as air pollutants. Conventional air emissions mitigation technologies such as scrubbers and selective catalytic reduction (SCR) systems can also mitigate emissions of by-product gases, but result in absorption or destruction of the by-product gas into a non-usable form, low-value non-circular product, or waste stream. For example, conventional SOXscrubbers used in flue gas desulfurization are wet or semi-dry processes that use limestone, lime, or seawater to scrub SOXgases and produce low-value gypsum by-products or acidic effluent. In another example, SCR systems for NOXremoval from flue gas streams utilize ammonia or urea as a reductant and produce N2and / or CO2gases that are typically non-monetizable. Such systems are prone toWSGR Docket No. 50741-727.601catalyst poisoning, require efficient particulate matter pre-filtration, are subject to additional permitting requirements for use of ammonia, and have potential to emit ammonia via “ammonia slip”, or the release of unreacted ammonia through the system.
[0132] With the disclosure described herein, emissions are reduced while recovering the byproduct gases in an integrated process that regenerates the initial precursors used to produce the mixed metal compound product. In some embodiments, the absorption process described in the disclosure is comparable or better than conventional mitigation technologies in reducing emissions.
[0133] In some embodiments, the absorption process is a modified liquid scrubber system, wherein the spent scrubber solution is directly reused in the integrated process, instead of disposal as an acidic waste stream or as a low value acid by-product as in a conventional liquid scrubber system. For example, Example 4 describes an absorber system that resembles conventional NOXscrubbers, but the resulting nitric acid produced is converted into a lithium nitrate solution in Example 8. Similarly, Example 6 describes a system similar to the sulfuric acid contact process for sulfuric acid production, but the resulting sulfuric acid stream is converted to a lithium sulfate solution in Example 9.
[0134] In some embodiments, the absorption process is an adaptation of conventional mitigation technologies, but where the liquid absorber solutions are modified to allow for easier conversion into a metal salt precursor or a metal precursor. For example, Example 5 utilizes a wet alkaline absorber similar to wet alkaline scrubbers described as potentially useful for production of sodium nitrite, but a lithium hydroxide solution is used instead of a sodium hydroxide solution to produce a lithium nitrite and lithium nitrate solution that is subsequently oxidized to produce a pure lithium nitrate stream in a single step.
[0135] In embodiments described above, the modification to the liquid scrubber system enable the facile and economic production a metal salt precursor, a metal precursor, or a combination of the two, which can be directly used as the input into a mixed metal oxide production process. By co-locating these two operations, an integrated processing system results, wherein the byproduct gases from the production of the mixed metal oxide are directly converted into the precursor used in the production of the same. This integration results in a more economical production of said mixed metal oxide, with the added benefit of reducing the emissions of byproduct gases.WSGR Docket No. 50741-727.601Integrated process
[0136] An aspect of the disclosure is the full integrated process that produces a mixed metal compound through a heat treatment of a mixture of a metal salt precursor and metal precursor, releases by-product gases that are absorbed and converted back to the metal salt precursor or metal precursor with minimal loss of the by-product gas.
[0137] In some embodiments, the output mixed metal compound product is Li4Ti5O12, the metal salt precursor is lithium nitrate, and the metal precursor is titanium dioxide. In these embodiments, the lithium nitrate metal salt precursor is supplied by absorption and conversion of NOXby-product gases produced by reaction of lithium nitrate with titanium dioxide; wherein the NOXis absorbed into a liquid and converted into lithium nitrate by reaction with a combination of lithium carbonate, lithium hydroxide and hydrogen peroxide. As such, in these embodiments, no lithium nitrate is supplied process, and the only inputs into the process are titanium dioxide, hydrogen peroxide, lithium carbonate, lithium hydroxide, and a small amount of nitric acid. This results in a more economical process than if lithium nitrate needed to be used as an input to the process. In some embodiments, about 99% of the NOXby-product gases are absorbed into an absorber solution containing hydrogen peroxide, forming an absorbed gas solution comprising nitric acid. In some embodiments, a small amount of nitric acid is dosed into the absorbed gas solution prior or during treatment and conversion to lithium nitrate to form the balance make-up of NOXgases that were not absorbed and released to atmosphere from the process. In such a process, about 99% of the lithium nitrate used in the production of Li4Ti5O12is a product of the recycled stream, with about 1% produced from conversion of fresh nitric acid.
[0138] In some embodiments, the output mixed metal compound product is Li4Ti5O12, the metal salt precursor is lithium sulfate, and the metal precursor is titanium dioxide. In these embodiments, the lithium sulfate metal salt precursor is supplied by absorption and conversion of SOXby-product gases produced by reaction of lithium sulfate with titanium dioxide; wherein the SOXis absorbed into a liquid and converted into lithium sulfate by reaction with a combination of lithium carbonate, lithium hydroxide and hydrogen peroxide. As such, in these embodiments, no lithium sulfate is supplied to the process, and the only inputs are titanium dioxide, hydrogen peroxide, lithium carbonate, lithium hydroxide, and a small amount of sulfuric acid. In some embodiments, about 99% of the SOXby-product gases are absorbed into an absorber solution containing hydrogen peroxide, forming an absorbed gas solution comprising sulfuric acid. In some embodiments, a small amount of sulfuric acid is dosed into the absorbed gas solution prior or during treatment and conversion to lithium sulfate to form the balance make-up of SOXgases that were not absorbed and released to atmosphere from theWSGR Docket No. 50741-727.601process. In such a process, about 99% of the lithium sulfate used in the production of Li4Ti5O12is a product of the recycled stream, with about 1% produced from conversion of fresh sulfuric acid.
[0139] In some embodiments, the output mixed metal compound product is Li4Mn5O12, the metal salt precursor is lithium nitrate, and the metal precursor is manganese dioxide. In these embodiments, the lithium nitrate metal salt precursor is supplied by absorption and conversion of NOXby-product gases produced by reaction of lithium nitrate with manganese dioxide; wherein the NOXis absorbed into a liquid and converted into lithium nitrate by reaction with a combination of lithium carbonate, lithium hydroxide and hydrogen peroxide. As such, in these embodiments, no lithium nitrate is supplied to the process, and the only inputs are manganese dioxide, hydrogen peroxide, lithium carbonate, lithium hydroxide, and a small amount of nitric acid. In some embodiments, about 99% of the NOXby-product gases are absorbed into an absorber solution containing hydrogen peroxide, forming an absorbed gas solution comprising nitric acid. In some embodiments, a small amount of nitric acid is dosed into the absorbed gas solution prior or during treatment and conversion to lithium nitrate to form the balance make-up of NOXgases that were not absorbed and released to atmosphere from the process. In such a process, about 99% of the lithium nitrate used in the production of Li4Mn5O12is a product of the recycled stream, with about 1% produced from conversion of fresh nitric acid.
[0140] In some embodiments, the output mixed metal compound product is Li4Mn5O12, the metal salt precursor is lithium sulfate, and the metal precursor is manganese dioxide. In these embodiments, the lithium sulfate metal salt precursor is supplied by absorption and conversion of SOXby-product gases produced by reaction of lithium sulfate with manganese dioxide; wherein the SOXis absorbed into a liquid and converted into lithium sulfate by reaction with a combination of lithium carbonate, lithium hydroxide and hydrogen peroxide. As such, in these embodiments, no lithium sulfate is supplied to the process, and the only inputs are manganese dioxide, hydrogen peroxide, lithium carbonate, lithium hydroxide, and a small amount of sulfuric acid. In some embodiments, about 99% of the SOXby-product gases are absorbed into an absorber solution containing hydrogen peroxide, forming an absorbed gas solution comprising sulfuric acid. In some embodiments, a small amount of sulfuric acid is dosed into the absorbed gas solution prior or during treatment and conversion to lithium sulfate to form the balance make-up of SOXgases that were not absorbed and released to atmosphere from the process. In such a process, about 99% of the lithium sulfate used in the production of Li4Mn5O12is a product of the recycled stream, with about 1% produced from conversion of fresh sulfuric acid.WSGR Docket No. 50741-727.601Sizing
[0141] In one aspect, provided herein are mixed metal compounds. In some embodiments, said mixed metal compounds are lithium selective sorbents. In some embodiments, said lithium selective sorbents are ion exchange materials. Further provided herein are methods of preparing such mixed metal compounds. In some embodiments, said methods comprise sizing a mixed metal compound. In some embodiments, the mixed metal compound is sized.
[0142] In some embodiments, sizing comprises a size reduction. In some embodiments, sizing comprises reducing average particle size. In some embodiments, sizing comprises controlling the average particle size, so that the size of the particles falls within an acceptable range. In some embodiments, sizing comprises treatment by milling.
[0143] In some embodiments, sizing comprises treatment in a crushing mill, a pin mill, a hammer mill, an impact mill, an air classifier mill, a jet mill, or a combination thereof. In some embodiments, sizing comprises treatment in a crushing mill. In some embodiments, the crushing mill comprises a disc mill, a jaw crushing mill, a roller mill, or a combination thereof.
[0144] In some embodiments, sizing provides a sized mixed metal compound with a d97 of about 2.5 microns to about 800 microns. In some embodiments, sizing mixed metal compound with a d97 of about 2.5 microns to about 70 microns. In some embodiments, sizing provides a sized mixed metal compound with a d97 of about 10 microns to about 150 microns. In some embodiments, sizing provides a sized mixed metal compound with a d97 of about 30 microns to about 800 microns. In some embodiments, sizing provides a sized mixed metal compound with a d97 of about 0.1 microns to about 0.5 microns. In some embodiments, sizing provides a sized mixed metal compound with a d97 of about 0.5 microns to about 1 microns. In some embodiments, sizing provides a sized mixed metal compound with a d97 of about 1 microns to about 5 microns. In some embodiments, sizing provides a sized mixed metal compound with a d97 of about 5 microns to about 10 microns. In some embodiments, sizing provides a sized mixed metal compound with a d97 of about 10 microns to about 20 microns. In some embodiments, sizing provides a sized mixed metal compound with a d97 of about 20 microns to about 30 microns. In some embodiments, sizing provides a sized mixed metal compound with a d97 of about 30 microns to about 40 microns. In some embodiments, sizing provides a sized mixed metal compound with a d97 of about 50 microns to about 75 microns. In some embodiments, sizing provides a sized mixed metal compound with a d97 of about 75 microns to about 100 microns. In some embodiments, sizing provides a sized mixed metal compound with a d97 of about 100 microns to about 250 microns. In some embodiments, sizing provides a sized mixed metal compound with a d97 of about 250 microns to about 500 microns. In someWSGR Docket No. 50741-727.601embodiments, sizing provides a sized mixed metal compound with a d97 of about 500 microns to about 1000 microns.
[0145] In some embodiments, sizing comprises treatment in a pin mill, a hammer mill, or an impact mill. In some embodiments, treatment in a pin mill, a hammer mill, or an impact mill provides a sized composite (e.g., the pre-calcined lithium selective sorbent composite following the sizing process and / or the lithium selective sorbent composite following the sizing process) with a d97 of about 30 microns to about 800 microns. In some embodiments, sizing comprises treatment in an air classifier mill. In some embodiments, treatment in an air classifier mill provides a sized composite (e.g., the pre-calcined lithium selective sorbent composite following the sizing process and / or the lithium selective sorbent composite following the sizing process) with a d97 of about 10 microns to about 150 microns. In some embodiments, sizing comprises treatment in a jet mill. In some embodiments, treatment in a jet mill provides a sized composite (e.g., the pre-calcined lithium selective sorbent composite following the sizing process and / or the lithium selective sorbent composite following the sizing process) with a d97 of about 2.5 microns to about 70 microns.
[0146] In some embodiments, the mixed metal compound provided following sizing is used for lithium extraction according to any embodiment of a method or system for lithium extraction (e.g., from a liquid resource) as described herein. The utility of the mixed metal compound provided herein is not limited to use according to the embodiments of methods and systems for lithium extraction described herein, particularly in view of the advantageous properties of such mixed metal compounds that are expounded throughout the present disclosure.Sieving
[0147] In one aspect, provided herein are mixed metal compounds. In some embodiments, said mixed metal compounds are lithium selective sorbents. In some embodiments, said lithium selective sorbents are ion exchange materials. Further provided herein are methods of preparing such mixed metal compounds. In some embodiments, said methods comprise sieving a mixed metal compound. In some embodiments, said methods comprise sieving the mixed metal compound.
[0148] In some embodiments, sieving removes particles from the mixed metal compound that are above a first size threshold, removes particles from the mixed metal compound that are below a second size threshold, or both. In some embodiments, sieving removes particles from the mixed metal compound that are above a size threshold. In some embodiments, sieving removes particles from the mixed metal compound that are below a size threshold. In someWSGR Docket No. 50741-727.601embodiments, sieving provides a mixed metal compound that comprises particles that are below a first size threshold, above a second size threshold, or both. In some embodiments, sieving provides a mixed metal compound that consists of particles that are below a first size threshold, above a second size threshold, or both. In some embodiments, sieving provides a mixed metal compound that consists of particles that are above a size threshold. In some embodiments, sieving provides a mixed metal compound that consists of particles that are below a size threshold. In some embodiments, the size threshold (e.g., the first size threshold, the second size threshold) is selected from: about 10 microns, about 20 microns, about 30 microns, about 40 microns, about 50 microns, about 60 microns, about 70 microns, about 80 microns, about 90 microns, about 100 microns, about 125 microns, about 150 microns, about 175 microns, about 200 microns, about 225 microns, about 250 microns, about 275 microns, about 300 microns, about 325 microns, about 350 microns, about 375 microns, about 400 microns, about 425 microns, about 450 microns, about 475 microns, about 500 microns, about 525 microns, about 550 microns, about 575 microns, about 600 microns, about 650 microns, about 700 microns, about 750 microns, about 800 microns, about 850 microns, about 900 microns, about 950 microns, about 1000 microns, about 1100 microns, about 1200 microns, about 1300 microns, about 1400 microns, and about 1500 microns. In some embodiments, sieving provides a mixed metal compound with a particle size of < 300 pm. In some embodiments, sieving provides a mixed metal compound with a particle size of > 300 pm. In some embodiments, sieving provides a mixed metal compound with a particle size of > 500 pm. In some embodiments, sieving provides a mixed metal compound with a particle size of > 1000 pm.
[0149] In some embodiments, sieving comprises dry sieving, wet sieving, sieving in the presence of air, sieving under vibration, or a combination thereof. In some embodiments, sieving comprises dry sieving. In some embodiments, sieving comprises wet sieving. In some embodiments, sieving comprises sieving under vibration. In some embodiments, sieving under vibration utilizes a vibratory sieve or a high energy vibratory sieve. In some embodiments, a vibratory sieve is utilized to sieve particles that are greater than about 300 microns in size. In some embodiments, a high energy vibratory sieve is utilized to sieve particles that are less than about 300 microns in size.
[0150] In some embodiments, sieving is conducted at a temperature of about 200 K to about 1000 K. In some embodiments, sieving is conducted at a temperature of about 200 K to about 500 K. In some embodiments, sieving is conducted at a temperature of about 500 K to about 750 K. In some embodiments, sieving is conducted at a temperature of about 750 K to about 1000 K.WSGR Docket No. 50741-727.601In some embodiments, sieving is conducted at a temperature of about 200 K, about 300 K, about 400 K, about 500 K, about 600 K, about 700 K, about 800 K about 900 K, or about 1000 K.
[0151] In some embodiments, the mixed metal compound provided following sieving is used for lithium extraction according to any embodiment of a method or system for lithium extraction (e.g., from a liquid resource) as described herein. The utility of the mixed metal compounds provided herein is not limited to use according to the embodiments of methods and systems for lithium extraction described herein, particularly in view of the advantageous properties of such mixed metal compounds that are expounded throughout the present disclosure.Properties of Mixed Metal Compounds
[0152] In one aspect, provided herein are mixed metal compounds. In some embodiments, said mixed metal compounds are lithium selective sorbents. In some embodiments, said lithium selective sorbents are ion exchange materials. Further provided herein are methods of preparing such mixed metal compounds. Described herein are some of the properties afforded by these mixed metal compounds.
[0153] In some embodiments, such mixed metal compounds have advantageous mechanical stability. In some embodiments, measurements of mechanical stability include bulk crush strength and attrition resistance. In some embodiments, the mixed metal compound has a bulk crush strength greater than 10 N / cm2. In some embodiments, the mixed metal compound has a bulk crush strength greater than about 10 N / cm2. In some embodiments, the mixed metal compound has a bulk crush strength greater than 10 N / cm2, 9 N / cm2, 8 N / cm2, 7 N / cm2, 6 N / cm2, or 5 N / cm2. In some embodiments, the mixed metal compound has a bulk crush strength of > 5 N / cm2, > 7.5 N / cm2, or > 10 N / cm2. In some embodiments, the bulk crush strength of the mixed metal compound is measured using ASTM D7084. In some embodiments, the mixed metal compound has an attrition resistance less than 7%. In some embodiments, the mixed metal compound has an attrition resistance less than about 7%. In some embodiments, the mixed metal compound has an attrition resistance less than about 8%, about 9%, about 10%, about 11%, about 12%, about 13%, about 14%, or about 15%. In some embodiments, the mixed metal compound has an attrition resistance < 12%, < 10%, or < 7%. In some embodiments, the attrition resistance of the mixed metal compound is measured using ASTM D4058.
[0154] In some embodiments, the advantageous mechanical stability of the mixed metal compound increases the service lifetime of the mixed metal compound, as compared to the lifetime of the mixed metal compound as a component of another construct or in isolation when used in methods for lithium extraction. Service lifetime can be quantified in terms of the numberWSGR Docket No. 50741-727.601of ion exchange cycles conducted before the mixed metal compound is replaced or permanently taken out of service. Service lifetime can be quantified in terms of the cumulative amount of lithium produced by the mixed metal compound before it is replaced or permanently taken out of service. In some embodiments, the advantageous mechanical stability of the mixed metal compound preserves the advantageous porosity of the mixed metal compound. In some embodiments, the advantageous mechanical stability of the mixed metal compound decreases the cost for producing a given quantity of lithium using direct lithium extraction from a liquid resource.
[0155] In one aspect, provided herein are mixed metal compounds. In some embodiments, such mixed metal compounds have advantageous porosity. In some embodiments, such advantageous porosity reduces the pressure drop across a packed bed of the mixed metal compound. In some embodiments, porosity is measured as surface area, total pore volume, average pore volume, pore size distribution, or a combination thereof.In some embodiments, the mixed metal compound has a surface area of about 10 m2 / g to about 100 m2 / g. In some embodiments, the mixed metal compound has a surface area of about 10 m2 / g to about 20 m2 / g, about 10 m2 / g to about 25 m2 / g, about 10 m2 / g to about 30 m2 / g, about 10 m2 / g to about 35 m2 / g, about 10 m2 / g to about 40 m2 / g, about 10 m2 / g to about 45 m2 / g, about 10 m2 / g to about 50 m2 / g, about 10 m2 / g to about 60 m2 / g, about 10 m2 / g to about 70 m2 / g, about 10 m2 / g to about 80 m2 / g, about 10 m2 / g to about 100 m2 / g, about 20 m2 / g to about 25 m2 / g, about 20 m2 / g to about 30 m2 / g, about 20 m2 / g to about 35 m2 / g, about 20 m2 / g to about 40 m2 / g, about 20 m2 / g to about 45 m2 / g, about 20 m2 / g to about 50 m2 / g, about 20 m2 / g to about 60 m2 / g, about 20 m2 / g to about 70 m2 / g, about 20 m2 / g to about 80 m2 / g, about 20 m2 / g to about 100 m2 / g, about 25 m2 / g to about 30 m2 / g, about 25 m2 / g to about 35 m2 / g, about 25 m2 / g to about 40 m2 / g, about 25 m2 / g to about 45 m2 / g, about 25 m2 / g to about 50 m2 / g, about 25 m2 / g to about 60 m2 / g, about 25 m2 / g to about 70 m2 / g, about 25 m2 / g to about 80 m2 / g, about 25 m2 / g to about 100 m2 / g, about 30 m2 / g to about 35 m2 / g, about 30 m2 / g to about 40 m2 / g, about 30 m2 / g to about 45 m2 / g, about 30 m2 / g to about 50 m2 / g, about 30 m2 / g to about 60 m2 / g, about 30 m2 / g to about 70 m2 / g, about 30 m2 / g to about 80 m2 / g, about 30 m2 / g to about 100 m2 / g, about 35 m2 / g to about 40 m2 / g, about 35 m2 / g to about 45 m2 / g, about 35 m2 / g to about 50 m2 / g, about 35 m2 / g to about 60 m2 / g, about 35 m2 / g to about 70 m2 / g, about 35 m2 / g to about 80 m2 / g, about 35 m2 / g to about 100 m2 / g, about 40 m2 / g to about 45 m2 / g, about 40 m2 / g to about 50 m2 / g, about 40 m2 / g to about 60 m2 / g, about 40 m2 / g to about 70 m2 / g, about 40 m2 / g to about 80 m2 / g, about 40 m2 / g to about 100 m2 / g, about 45 m2 / g to about 50 m2 / g, about 45 m2 / g to about 60 m2 / g, about 45 m2 / g to about 70 m2 / g, about 45 m2 / g to about 80 m2 / g, about 45 m2 / g to about 100 m2 / g, about 50WSGR Docket No. 50741-727.601m2 / g to about 60 m2 / g, about 50 m2 / g to about 70 m2 / g, about 50 m2 / g to about 80 m2 / g, about 50 m2 / g to about 100 m2 / g, about 60 m2 / g to about 70 m2 / g, about 60 m2 / g to about 80 m2 / g, about 60 m2 / g to about 100 m2 / g, about 70 m2 / g to about 80 m2 / g, about 70 m2 / g to about 100 m2 / g, or about 80 m2 / g to about 100 m2 / g. In some embodiments, the mixed metal compound has a surface area of about 10 m2 / g, about 20 m2 / g, about 25 m2 / g, about 30 m2 / g, about 35 m2 / g, about 40 m2 / g, about 45 m2 / g, about 50 m2 / g, about 60 m2 / g, about 70 m2 / g, about 80 m2 / g, or about 100 m2 / g. In some embodiments, the mixed metal compound has a surface area of at least about 10 m2 / g, about 20 m2 / g, about 25 m2 / g, about 30 m2 / g, about 35 m2 / g, about 40 m2 / g, about 45 m2 / g, about 50 m2 / g, about 60 m2 / g, about 70 m2 / g, or about 80 m2 / g. In some embodiments, the mixed metal compound has a surface area of at most about 20 m2 / g, about 25 m2 / g, about 30 m2 / g, about 35 m2 / g, about 40 m2 / g, about 45 m2 / g, about 50 m2 / g, about 60 m2 / g, about 70 m2 / g, about 80 m2 / g, or about 100 m2 / g.
[0156] In some embodiments, the mixed metal compound has a total pore volume of about 0.001 mL / g to about 0.1 mL / g. In some embodiments, the mixed metal compound has a total pore volume of about 0.001 mL / g to about 0.005 mL / g, about 0.001 mL / g to about 0.008 mL / g, about 0.001 mL / g to about 0.01 mL / g, about 0.001 mL / g to about 0.015 mL / g, about 0.001 mL / g to about 0.018 mL / g, about 0.001 mL / g to about 0.02 mL / g, about 0.001 mL / g to about 0.05 mL / g, about 0.001 mL / g to about 0.06 mL / g, about 0.001 mL / g to about 0.07 mL / g, about 0.001 mL / g to about 0.08 mL / g, about 0.001 mL / g to about 0.1 mL / g, about 0.005 mL / g to about 0.008 mL / g, about 0.005 mL / g to about 0.01 mL / g, about 0.005 mL / g to about 0.015 mL / g, about 0.005 mL / g to about 0.018 mL / g, about 0.005 mL / g to about 0.02 mL / g, about 0.005 mL / g to about 0.05 mL / g, about 0.005 mL / g to about 0.06 mL / g, about 0.005 mL / g to about 0.07 mL / g, about 0.005 mL / g to about 0.08 mL / g, about 0.005 mL / g to about 0.1 mL / g, about 0.008 mL / g to about 0.01 mL / g, about 0.008 mL / g to about 0.015 mL / g, about 0.008 mL / g to about 0.018 mL / g, about 0.008 mL / g to about 0.02 mL / g, about 0.008 mL / g to about 0.05 mL / g, about 0.008 mL / g to about 0.06 mL / g, about 0.008 mL / g to about 0.07 mL / g, about 0.008 mL / g to about 0.08 mL / g, about 0.008 mL / g to about 0.1 mL / g, about 0.01 mL / g to about 0.015 mL / g, about 0.01 mL / g to about 0.018 mL / g, about 0.01 mL / g to about 0.02 mL / g, about 0.01 mL / g to about 0.05 mL / g, about 0.01 mL / g to about 0.06 mL / g, about 0.01 mL / g to about 0.07 mL / g, about 0.01 mL / g to about 0.08 mL / g, about 0.01 mL / g to about 0.1 mL / g, about 0.015 mL / g to about 0.018 mL / g, about 0.015 mL / g to about 0.02 mL / g, about 0.015 mL / g to about 0.05 mL / g, about 0.015 mL / g to about 0.06 mL / g, about 0.015 mL / g to about 0.07 mL / g, about 0.015 mL / g to about 0.08 mL / g, about 0.015 mL / g to about 0.1 mL / g, about 0.018 mL / g to about 0.02 mL / g, about 0.018 mL / g to about 0.05 mL / g, about 0.018 mL / g to about 0.06 mL / g, about 0.018 mL / g to about 0.07WSGR Docket No. 50741-727.601mL / g, about 0.018 mL / g to about 0.08 mL / g, about 0.018 mL / g to about 0.1 mL / g, about 0.02 mL / g to about 0.05 mL / g, about 0.02 mL / g to about 0.06 mL / g, about 0.02 mL / g to about 0.07 mL / g, about 0.02 mL / g to about 0.08 mL / g, about 0.02 mL / g to about 0.1 mL / g, about 0.05 mL / g to about 0.06 mL / g, about 0.05 mL / g to about 0.07 mL / g, about 0.05 mL / g to about 0.08 mL / g, about 0.05 mL / g to about 0.1 mL / g, about 0.06 mL / g to about 0.07 mL / g, about 0.06 mL / g to about 0.08 mL / g, about 0.06 mL / g to about 0.1 mL / g, about 0.07 mL / g to about 0.08 mL / g, about 0.07 mL / g to about 0.1 mL / g, or about 0.08 mL / g to about 0.1 mL / g. In some embodiments, the mixed metal compound has a total pore volume of about 0.001 mL / g, about 0.005 mL / g, about 0.008 mL / g, about 0.01 mL / g, about 0.015 mL / g, about 0.018 mL / g, about 0.02 mL / g, about 0.05 mL / g, about 0.06 mL / g, about 0.07 mL / g, about 0.08 mL / g, or about 0.1 mL / g. In some embodiments, the mixed metal compound has a total pore volume of at least about 0.001 mL / g, about 0.005 mL / g, about 0.008 mL / g, about 0.01 mL / g, about 0.015 mL / g, about 0.018 mL / g, about 0.02 mL / g, about 0.05 mL / g, about 0.06 mL / g, about 0.07 mL / g, or about 0.08 mL / g. In some embodiments, the mixed metal compound has a total pore volume of at most about 0.005 mL / g, about 0.008 mL / g, about 0.01 mL / g, about 0.015 mL / g, about 0.018 mL / g, about 0.02 mL / g, about 0.05 mL / g, about 0.06 mL / g, about 0.07 mL / g, about 0.08 mL / g, or about 0.1 mL / g.
[0157] In some embodiments, the mixed metal compound comprises micropores, mesopores, and macropores with diameters ranging between about 5 Ångstroms and 10 microns.
[0158] In some embodiments, the mixed metal compound has a pore size distribution with a characteristic D50 value. The parameter D50 specifies that 50% of the pores are larger than the specified value, and 50% of the pores are smaller than the specified value. In some embodiments, the D50 value is about 1 mm. In some embodiments, the D50 value is about 2 mm. In some embodiments, the D50 value is from about 0.4 mm to about 3 mm. In some embodiments, the D50 value is from about 1 mm to about 10 mm. In some embodiments, the D50 value is about 0.4 mm, about 1 mm, about 2 mm, about 3 mm, about 4 mm, about 5 mm, about 6 mm, about 7 mm, about 8 mm, about 9 mm, or about 10 mm. In some embodiments, the D50 value is from about 70 microns to about 700 microns. In some embodiments, the D50 value is from about 10 microns to about 70 microns. In some embodiments, the D50 value is from about 1 microns to about 10 microns. In some embodiments, the D50 value is from about 0.1 microns to about 1 microns.
[0159] In some embodiments, liquids (e.g., a liquid resource, brine, an acidic solution) are flowed through a packed bed of the mixed metal compound. In some embodiments, the advantageous porosity of the mixed metal compound reduces the pressure required to flowWSGR Docket No. 50741-727.601liquids through the packed bed. In some embodiments, the pressure required to flow liquids through the packed bed is less than 10 psi, less than 9 psi, less than 8 psi, less than 7 psi, less than 6 psi, less than 5 psi, less than 4 psi, less than 3 psi, less than 2 psi, or less than 1 psi. In some embodiments, the flow distance through the packed bed is about 10 cm, about 25 cm, about 50 cm, about 75 cm, about 100 cm, about 200 cm, about 300 cm, about 400 cm, about 500 cm, about 600 cm, about 700 cm, about 800 cm, about 900 cm, about 1 meter, about 1.5 meters, about 2 meters, or more than 2 meters. In some embodiments, the flow distance through the packed bed is less than about 1 meter. In some embodiments, the flow distance through the packed bed is greater than about 1 meter. In some embodiments, the flow distance through the packed bed is coincident (i.e., aligns with) with the longest dimension of the packed bed. In some embodiments, the flow distance through the packed bed is orthogonal (i.e., perpendicular) to the longest dimension of the packed bed. In some embodiments, a mixed metal compound with a larger particle size is selected to further reduce the pressure required to flow liquids through the packed bed.
[0160] In some embodiments of the lithium extraction process, during ion exchange, binders bound to the surface of the mixed metal compound limit mass transport due to the low surface area and low porosity observed with existing ion exchange bead manufacturing methods. In some embodiments described herein, the high surface areas and high porosities achieved through the use of binders and pore forming processes described herein, allow larger particle sizes and additional particle morphologies, leading to advantageous mass transport of lithium and protons to and from the mixed metal compound, leading to increased performance in lithium extraction.
[0161] In some embodiments, the advantageous porosity of the mixed metal compound increases the rate of lithium uptake from solution by the mixed metal compound within the mixed metal compound. In some embodiments, the advantageous porosity of the mixed metal compound increases the purity of lithium produced by methods of lithium extraction that utilize the mixed metal compound. In some embodiments, the advantageous porosity of the mixed metal compound decreases the cost for producing a given quantity of lithium using direct lithium extraction from a liquid resource. In some embodiments, the advantageous porosity of the mixed metal compound increases the diffusion of lithium to and from the active surface of the mixed metal compound. In some embodiments, the advantageous porosity of the lithium sorbent composite increases the diffusion of protons to and from the active surface of the mixed metal compound. In some embodiments, the advantageous porosity of the mixed metal compound increases the effectiveness factor for utilization of mixed metal compound. In someWSGR Docket No. 50741-727.601embodiments, the advantageous porosity of the mixed metal compound increases utilization of mixed metal compound for lithium absorption and elution.
[0162] In some embodiments, the advantageous surface area of the mixed metal compound increases the rate of lithium uptake from solution by the mixed metal compound within the mixed metal compound. In some embodiments, the advantageous surface area of the mixed metal compound increases the purity of lithium produced by methods of lithium extraction that utilize the mixed metal compound. In some embodiments, the advantageous surface area of the mixed metal compound decreases the cost for producing a given quantity of lithium using direct lithium extraction from a liquid resource. In some embodiments, the advantageous surface area of the mixed metal compound increases the diffusion of lithium to and from the active surface of the mixed metal compound. In some embodiments, the advantageous surface area of the mixed metal compound increases the diffusion of protons to and from the active surface of the mixed metal compound. In some embodiments, the advantageous surface area of the mixed metal compound increases the effectiveness factor for utilization of mixed metal compound. In some embodiments, the advantageous surface area of the mixed metal compound increases utilization of mixed metal compound for lithium absorption and elution.
[0163] In one aspect, provided herein are mixed metal compounds. In some embodiments, such mixed metal compounds have advantageous chemical stability. In some embodiments, said advantageous chemical stability preserves the advantageous porosity of the mixed metal compound. In some embodiments, said advantageous chemical stability leads to a minimal dissolution of the lithium selective sorbent, the binder, or both when the mixed metal compound is used in a method of lithium extraction. In some embodiments, said advantageous chemical stability leads to a minimal dissolution of the lithium selective sorbent, the binder, or both when the mixed metal compound is contacted to an acidic solution.Lithium Selective Sorbents, Including Ion Exchange Materials, Obtained from Mixed Metal Compounds
[0164] In an aspect, disclosed herein are methods and systems for production of a mixed metal compound. In an aspect, said mixed metal oxide is a lithium selective sorbent. In some embodiments, said lithium selective sorbent comprises lithium. In some embodiments, said lithium selective sorbent comprises a lithium and an oxide. In some embodiments, said lithium selective sorbent comprises a lithium and an oxide, wherein said oxide is selected from an oxide of titanium (Ti), an oxide of iron (Fe), an oxide of tin (Sn), an oxide of manganese (Mn), anWSGR Docket No. 50741-727.601oxide of copper (Cu), an oxide of aluminum (Al), an oxide of niobium (Nb), or mixtures or combinations thereof.
[0165] In an aspect, disclosed herein are methods and systems for production of a mixed metal oxide, wherein said oxide comprises a mixture of a first metal, a second metal, and an optional third or more metals; wherein the first metal is selected from lithium or sodium; wherein the second metal is selected from titanium, iron, tin, manganese, copper, aluminum, or niobium; and wherein the third or more metals are optionally selected from but different to the first or second metals. In an aspect, disclosed herein are methods and systems for production of a mixed metal oxide, wherein said oxide is a lithium selective sorbent comprising a mixture of a first metal, a second metal, and an optional third or more metals; wherein the first metal is selected from lithium or sodium; wherein the second metal is selected from titanium, iron, tin, manganese, copper, aluminum, or niobium; and wherein the third or more metals are optionally selected from but different to the first or second metals. In an aspect, disclosed herein are methods and systems for production of a mixed metal oxide, wherein said oxide is a lithium selective sorbent comprising a mixture of lithium, a second metal, and an optional third or more metals; wherein the second metal is selected from titanium, iron, tin, manganese, copper, aluminum, or niobium; and wherein the third or more metals are optionally selected from but different to the first or second metals.
[0166] In an aspect, disclosed herein are methods and systems for lithium recovery from a liquid resource. In an aspect, a lithium selective sorbent is utilized to selective extract lithium from a liquid sorbent. In one aspect, said lithium selective sorbent is an ion exchange material. In an aspect, disclosed herein are methods and systems that utilize a lithium-selective ion exchange material to recover lithium from a liquid resource. The nonlimiting embodiments described below describe methods and system for recovery of lithium utilizing a lithium selective sorbent, which are understood to apply to the mixed metal compounds produced by the disclosure described herein.
[0167] In some embodiments, a lithium selective sorbent is formed into ion exchange beads. In some embodiments, said beads are porous beads. In some embodiments, said beads are used for lithium extraction. In some embodiments, a mixed metal compound is a lithium selective ion exchange material, which is formed into ion exchange beads. Therefore, it will be understood that all characteristics and properties described herein for mixed metal compounds, lithium selective sorbents, ion exchange materials, or lithium selective ion exchange materials apply to beads formed from the same.WSGR Docket No. 50741-727.601
[0168] In some embodiments, lithium selective sorbent composites are formed into a bead, said bead comprising an ion exchange material. Therefore, embodiments described herein for “ion exchange beads” should be understood to apply to any embodiments for “ion exchange material”, or for any material composition comprising an ion exchange material, including but not limited to coated ion exchange material(s), beads comprising coated ion exchange material(s), ion exchange materials embedded in a structural support, ion exchange materials embedded in a matrix, composites comprising ion exchange material(s), lithium selective sorbent composites - wherein the lithium selective sorbent comprises an ion exchange material, or combinations thereof.
[0169] In some embodiments, producing a lithium product from a liquid resource comprises lithium recovery. In some embodiments, a system, a method, or a process for lithium recovery from a liquid resource may be employed in a system, a method, or a process for producing a lithium product from a liquid resource. In some embodiments, the methods and systems disclosed herein utilize ion exchange materials. In some embodiments, the lithium selective sorbent comprises an ion exchange material. In some embodiments, an ion exchange material is utilized in a variety of forms or as a constituent of a construct that comprises one or more ion exchange materials (e.g., a lithium selective sorbent composite). In some embodiments, an ion exchange material is utilized in a form that specifically enables or optimizes the performance of the method or system in which the ion exchange material is utilized. In some embodiments, an ion exchange material is utilized as a constituent of a construct that specifically enables or optimizes the performance of the method or system in which the ion exchange material is utilized. In some embodiments, ion exchange materials are coated.
[0170] In some embodiments, ion exchange material is in the form of ion exchange particles. In some embodiments, ion exchange material is in the form of uncoated ion exchange particles. In some embodiments, ion exchange material is in the form of coated ion exchange particles. In some embodiments, ion exchange particles are coated or uncoated. In some embodiments, ion exchange particles are utilized as a mixture that comprises coated ion exchange particles and uncoated ion exchange particles. In some embodiments, ion exchange particles comprise one or more ion exchange materials. In some embodiments, ion exchange particles comprise a lithiumselective sorbent.
[0171] In some embodiments, lithium selective sorbent composites are a construct that comprises ion exchange material that can be used according to the methods and systems described herein. In some embodiments, lithium selective sorbent composites comprise ion exchange material. In some embodiments, the ion exchange material is coated or uncoated. InWSGR Docket No. 50741-727.601some embodiments, the lithium selective sorbent composites are porous. In some embodiments, lithium selective sorbent composites comprise one or more ion exchange materials. In some embodiments, lithium selective sorbent composites comprise a lithium-selective sorbent.
[0172] In some embodiments, lithium selective sorbent composites have diameters less than about one millimeter, contributing to a high pressure difference across a packed bed of lithium selective sorbent composite as a liquid resource and other fluids are pumped through the packed bed by application of an appropriate force. To minimize pressure across the packed bed of lithium selective sorbent composite and to minimize the associated appropriate force and amount of energy associated with applying said appropriate force, vessels with optimized geometries can be used to reduce the flow distance through the packed bed of lithium selective sorbent composite. These vessels can be networked with pH modulation units to achieve adequate control of the pH of the liquid resource.
[0173] In some embodiments, a network of vessels loaded with lithium selective sorbent composite comprises two vessels, three vessels, four vessels, five vessels, six vessels, seven vessels, eight vessels, nine vessels, 10 vessels, 11 vessels, 12 vessels, 13-14 vessels, 15-20 vessels, 20-30 vessels, 30-50 vessels, 50-70 vessels, 70-100 vessels, or more than 100 vessels.
[0174] In some embodiments, ion exchange material, or a form thereof, or a construct comprised thereof, is loaded into an ion exchange device described herein. In some embodiments, an ion exchange device comprises a column, tank, or vessel. In some embodiments, an ion exchange device is a component of a system for lithium recovery from a liquid resource. Alternating flows of liquid resource, eluent, and other process fluids are optionally flowed through an ion exchange device to extract lithium from the liquid resource and produce a synthetic lithium solution, which is eluted from the ion exchange device using an eluent. As liquid resource flows through the ion exchange device, the ion exchange material absorb lithium while releasing hydrogen, where both the lithium and hydrogen are cations. After the ion exchange material have absorbed lithium, an eluent is used to elute the lithium from the ion exchange material to produce a lithium eluate. A lithium eluate can be a synthetic lithium solution according to some embodiments. In some embodiments, an eluent comprises acid or an acid eluent.
[0175] Lithium is an essential element for batteries and other technologies. Lithium is found in a variety of liquid resources, including natural and synthetic brines and leachate solutions from minerals, clays, and recycled products. Lithium can be extracted from such liquid resources using an ion exchange process that utilizes ion exchange materials. In some embodiments, lithium selective sorbent composites comprise ion exchange materials in addition to otherWSGR Docket No. 50741-727.601components. In some embodiments, lithium selective sorbent composites are utilized in methods for lithium recovery and systems for lithium recovery. Ion exchange materials can absorb lithium from a liquid resource while releasing hydrogen, and then elute lithium in acid while absorbing hydrogen. In methods for lithium recovery from a liquid resource, the ion exchange process can be repeated to extract lithium from a liquid resource and yield a synthetic lithium solution. The synthetic lithium solution can be further processed into chemicals for the battery industry or other industries.
[0176] In some embodiments, ion exchange particles comprise ion exchange materials. Ion exchange particles can be in the form of small particles, which together constitute a fine powder. Small sizes of ion exchange particles may be required to minimize the diffusion distance that lithium must travel to reach the core of the ion exchange particles and ensure the entirety of the ion exchange material within the ion exchange particle is utilized in the course of an ion exchange process or method for lithium recovery. In some cases, ion exchange particles are coated with coating materials that can minimize dissolution of the ion exchange particles while allowing efficient transfer of lithium and hydrogen to and from the ion exchange particles.
[0177] One major challenge for methods of lithium recovery from a liquid resource that comprise use of ion exchange particles is the loading of the ion exchange particles into an ion exchange device in such a way that liquid resource and acid flow through the ion exchange device with minimal clogging. One major challenge for methods of lithium recovery from a liquid resource that comprise use of ion exchange particles is the loading of the ion exchange particles into an ion exchange device in such a way that liquid resource and acid flow through the ion exchange device with minimal pressure drop. Thus, ion exchange material and / or ion exchange particles can be formed into lithium selective sorbent composite that can be loaded into an ion exchange device. In some embodiments, lithium selective sorbent composite comprises ion exchange materials in addition to other components and can be utilized in methods for lithium recovery and systems for lithium recovery. The lithium selective sorbent composite, as loaded into an ion exchange device, can be loaded such that void spaces are present between the lithium selective sorbent composite, and these void spaces can facilitate flow of liquids through the column. In some embodiments, a flow is initiated, modulated, or terminated by pumping. In some embodiments, the lithium selective sorbent composite hold their constituent ion exchange particles in place and prevent free movement of ion exchange particles throughout the ion exchange device.
[0178] When ion exchange material is formed into lithium selective sorbent composite, the penetration of liquid resource and acid into the lithium selective sorbent composite byWSGR Docket No. 50741-727.601convection and diffusion can become unacceptably slow. A slow rate of convection and diffusion of the acid and liquid resource into the lithium selective sorbent composite can slow the kinetics of lithium absorption and release thereby. Slow kinetics of lithium absorption and release can create problems for the operation of an ion exchange device. Slow kinetics of lithium absorption and release can consequently require correspondingly slow flow rates through an ion exchange device. Slow kinetics of lithium absorption and release can also lead to low lithium recovery from the liquid resource and inefficient use of acid to elute the lithium according to the methods and systems described herein.
[0179] In some embodiments, the lithium selective sorbent composites comprise networks of pores that facilitate the transport of liquids flowed through an ion exchange device into lithium selective sorbent composites. The geometry and physical dimensions of pore networks in lithium selective sorbent composites can be strategically controlled to allow for faster and more complete access of liquid resource, washing water, acid, and other process fluids into the interior of the ion exchange material. Faster and more complete access of liquid resource, washing water, acid, and other process fluids into the interior of the lithium selective sorbent composites leads to a more effective delivery lithium and hydrogen to the ion exchange material therein. More effective delivery of lithium and hydrogen to the ion exchange material within lithium selective sorbent composites can lead to greater lithium recovery according to the methods and systems described herein.
[0180] Another challenge to consider and overcome in a method or system for lithium recovery from a liquid resource using ion exchange materials is the undesired dissolution and degradation of the ion exchange materials. Undesired dissolution and degradation of the ion exchange materials can occur during a step comprising lithium elution from the ion exchange material in acid. Undesired dissolution and degradation of the ion exchange materials can occur during a step comprising lithium extraction from a liquid resource by the ion exchange material. In some embodiments, to yield a synthetic lithium solution from the ion exchange process it is desirable to use a concentrated acid solution as an acid eluent in a step comprising lithium elution from the ion exchange material. However, concentrated acid solutions dissolve and degrade ion exchange materials, which can decrease the performance and useful lifetime of the materials. Therefore, in some embodiments the lithium selective sorbent composites contain coated ion exchange particles that are comprised of an ion exchange material and a coating material. The coating material can protect the ion exchange material from undesired dissolution and degradation during lithium elution from the ion exchange material into acid, during lithium uptake from a liquid resource into the ion exchange material, and during other steps of an ionWSGR Docket No. 50741-727.601exchange process according to the methods and systems described herein. In some embodiments, use of lithium selective sorbent composites that comprise coated ion exchange particles allows for the use of a concentrated acid as an acid eluent to yield a synthetic lithium solution.
[0181] In one aspect described herein, an ion exchange material is selected for use in lithium selective sorbent composites based on one or more properties of the ion exchange material. In some embodiments, desirable properties of the ion exchange material comprise high lithium absorption capacity, high selectivity for lithium extraction from a liquid resource relative to extraction of other ions such as sodium and magnesium, strong lithium uptake in liquid resources including those with low concentrations of lithium, facile elution of lithium with a small excess of acid, fast ionic diffusion throughout the ion exchange material, combinations thereof, and sub-combinations thereof. In one aspect described herein, a coating material is selected for use as a coating for ion exchange particles based on its ability to prevent undesirable dissolution and chemical degradation of the ion exchange particles during lithium elution from the ion exchange particles in acid and also during lithium uptake by the ion exchange particles from liquid resources.
[0182] In some embodiments, wherein lithium selective sorbent composites are used in an ion exchange device, the liquid resource containing lithium is flowed through the ion exchange device so that the lithium selective sorbent composites absorb lithium from the liquid resource while releasing hydrogen. After the lithium selective sorbent composites have absorbed lithium, an acid is pumped through the ion exchange device so that the lithium selective sorbent composites release lithium into the acid while absorbing hydrogen. In some embodiments, the ion exchange device is operated in a co-flow mode wherein the liquid resource and acid are alternately flowed through the ion exchange device in the same direction. In some embodiments, the ion exchange device is operated in counter-flow mode wherein the liquid resource and acid are alternately flowed through the ion exchange device in opposite directions. In some embodiments, in between flows of the liquid resource and flows of acid, water or other solutions is flowed through the ion exchange device for purposes such as adjusting pH in the ion exchange device or removing potential contaminants. In some embodiments, lithium selective sorbent composites form a fixed bed or a moving bed, wherein the moving bed can move in a direction opposed to the flows of liquid resource and acid. In some embodiments, lithium selective sorbent composites are moved between multiple ion exchange devices, wherein the lithium selective sorbent composites form a moving bed that can be transferred from one ion exchange device to another. In some embodiments, lithium selective sorbent composites are movedWSGR Docket No. 50741-727.601between multiple ion exchange devices, wherein different ion exchange devices are independently configured to accommodate a flow of liquid resource, a flow of acid, a flow of water, or a flow of another process fluid. In some embodiments, before or after the liquid resource is flowed through an ion exchange device, the liquid resource is subjected to other processes including other ion exchange processes, solvent extraction, evaporation, chemical treatment, precipitation to remove lithium, precipitation to remove other chemical species, or to otherwise treat the liquid resource.
[0183] In some embodiments, wherein ion exchange particles are used in an ion exchange device, the liquid resource containing lithium is flowed through the ion exchange device so that the ion exchange particles absorb lithium from the liquid resource while releasing hydrogen. After the ion exchange particles have absorbed lithium, an acid is pumped through the ion exchange device so that the ion exchange particles release lithium into the acid while absorbing hydrogen. In some embodiments, the ion exchange device is operated in a co-flow mode wherein the liquid resource and acid are alternately flowed through the ion exchange device in the same direction. In some embodiments, the ion exchange device is operated in counter-flow mode wherein the liquid resource and acid are alternately flowed through the ion exchange device in opposite directions. In some embodiments, in between flows of the liquid resource and flows of acid, water or other solutions are flowed through the ion exchange device for purposes such as adjusting pH in the ion exchange device or removing potential contaminants. In some embodiments, ion exchange particles form a fixed bed or a moving bed, wherein the moving bed can move in a direction opposed to the flows of liquid resource and acid. In some embodiments, ion exchange particles are moved between multiple ion exchange devices, wherein the ion exchange particles form a moving bed that can be transferred from one ion exchange device to another. In some embodiments, ion exchange particles are moved between multiple ion exchange devices, wherein different ion exchange devices are independently configured to accommodate a flow of liquid resource, a flow of acid, a flow of water, or a flow of another process fluid. In some embodiments, before or after the liquid resource is flowed through an ion exchange device, the liquid resource is subjected to other processes including other ion exchange processes, solvent extraction, evaporation, chemical treatment, precipitation to remove lithium, precipitation to remove other chemical species, or to otherwise treat the liquid resource.
[0184] In some embodiments, when ion exchange material is treated with acid a synthetic lithium solution is produced. In some embodiments, the synthetic lithium solution is further processed to produce lithium chemicals. In some embodiments, lithium chemicals produced from synthetic lithium solutions are provided for an industrial application. In someWSGR Docket No. 50741-727.601embodiments, lithium chemicals produced from synthetic lithium solutions are further processed to produce one or more alternative lithium chemicals that are contemplated for use in an application for which the one or more alternative lithium chemicals is better suited as compared to the lithium chemicals.
[0185] In some embodiments, the lithium selective sorbent is a protonated ion exchange material or an adsorbent. In some embodiments, said protonated ion exchange material is generated by treating a pre-activated ion exchange material with an acid. In some embodiments, said pre-activated ion exchange material comprises LiFePCh, LiMnPO4U, Li2MTiOs, Li2MnO3, Li2SnO3, Li4Ti5O12, Li4Mn5O12, LiMmCL, Li1.6Mn1.6O4, LiAlO2, LiCuO2, LiTiO2, Li4TiO4, Li7Ti11O24, Li3VO4, Li2Si3O7, Li2CuP2O7, modifications thereof, solid solutions thereof, or a combination thereof. In some embodiments, said lithium selective sorbent is an adsorbent. In some embodiments, the adsorbent comprises a crystalline lithium salt aluminate, a lithium aluminum intercalate, LiCl·2Al(OH)3, crystalline aluminum trihydroxide (Al(OH)3), gibbsite, beyerite, nordstrandite, alumina hydrate, bauxite, amorphous aluminum trihydroxide, activated alumina layered lithium-aluminum double hydroxides, Li A12(OH)eCl, combinations thereof, compounds thereof, or solid solutions thereof. In some embodiments, the adsorbent comprises a lithium aluminum intercalate. In some embodiments, said pre-activated ion exchange material comprises a mixed metal compound prepared according to any one of the methods for preparing a mixed metal compound described in the present disclosure.
[0186] In some embodiments, a pre-activated ion exchange material is selected from the following list: an oxide, a phosphate, an oxyfluoride, a fluorophosphate, or combinations thereof. In some embodiments, an oxide, a phosphate, an oxyfluoride, a fluorophosphate, or combinations thereof independently further comprise: (i) lithium, and (ii) manganese or titanium. In some embodiments, the ion exchange material is an oxide that further comprises: (i) lithium, and (ii) manganese or titanium. In some embodiments, the pre-activated ion exchange material is selected from the following list: Li4Mn5O12, Li4Ti5O12, Li2MC>3 (M = Ti, Mn, Sn), LiMn2O4, Li1.6Mn1.6O4, LiMCh (M = Al, Cu, Ti), Li4TiO4, Li7Ti11O24, LisVCL, Li2Si3O?, LiFePO4, LiMnPO4, Li2CuP2O7, A1(OH)3, LiCl.xAl(OH)3.yH2O, SnO2.xSb2O5.yH2O, TiO2.xSb2O5.yH2O, solid solutions thereof, or combinations thereof. In some embodiments, the pre-activated ion exchange material is selected from the following list: Li4Mn5O12, Li4Ti5O12, Li1.6Mn1.6O4, Li2MO3 (M = Ti, Mn, Sn), LiFePO4, solid solutions thereof, or combinations thereof.
[0187] In some embodiments, a coating material used to form a coating on the lithium selective sorbent. In some embodiments, a coating material used to form a coating on an ion exchangeWSGR Docket No. 50741-727.601material or on ion exchange particles that comprise an ion exchange material is selected from the following list: a carbide, a nitride, an oxide, a phosphate, a fluoride, a polymer, carbon, a carbonaceous material, or combinations thereof. In some embodiments, the coating material comprises an oxide different from the oxide of the ion exchange material. In some embodiments, a coating material is selected from the following list: TiCh, ZrCh, MoO?, SnCh, Nb20s, Ta20s, SiC>2, Li2TiO3, Li2ZrOs, Li2SiOs, Li2MnO3, Li2MoOs, LiNbCh, LiTaCh, AIPO4, LaPC>4, ZrP2O?, MOP2O7, MO2P3O12, BaSO4, AIF3, SiC, TiC, ZrC, SisN4, ZrN, BN, carbon, graphitic carbon, amorphous carbon, hard carbon, diamond-like carbon, solid solutions thereof, or combinations thereof. In some embodiments, a coating material is selected from the following list: TiCh, ZrCh, MoO2, SiCh, Li2TiC>3, Li2ZrO3, Li2SiO3, Li2MnO3, LiNbCh, AIF3, SiC, SisN4, graphitic carbon, amorphous carbon, diamond-like carbon, or combinations thereof.
[0188] In some embodiments, the ion exchange particles have an average diameter that is selected from the following list: less than 10 nm, less than 100 nm, less than 1,000 nm, less than 10,000 nm, or less than 100,000 nm. In some embodiments, the ion exchange particles have an average size that is selected from the following list: less than 200 nm, less than 2,000 nm, or less than 20,000 nm.
[0189] It is recognized that measurements of average particle diameter can vary according to the method of determination utilized. Determination of said average particle diameter according to one method to obtain one or more values shall be understood to inherently encompass all other values that may be obtained using other methods. The average particle diameter can be determined using sieve analysis. The average particle diameter can be determined using optical microscopy. The average particle diameter can be determined using electron microscopy. The average particle diameter can be determined using laser diffraction. In some embodiments, the average particle diameter is determined using laser diffraction, wherein a Bettersizer ST instrument is used. In some embodiments, the average particle diameter is determined using a Bettersizer ST instrument. In some embodiments, the average particle diameter is determined using laser diffraction, wherein an Anton-Parr particle size analyzer (PSA) instrument is used. In some embodiments, the average particle diameter is determined using an Anton-Parr PSA instrument. The average particle diameter can be determined using dynamic light scattering. The average particle diameter can be determined using static image analysis. The average particle diameter can be determined using dynamic image analysis.
[0190] In some embodiments, the ion exchange particles are secondary particles comprised of smaller primary particles that have an average diameter selected from the following list: lessWSGR Docket No. 50741-727.601than 10 nm, less than 100 nm, less than 1,000 nm, or less than 10,000 nm. In some embodiments, smaller primary particles comprise an ion exchange material.
[0191] In some embodiments, the ion exchange material or the ion exchange particles comprising an ion exchange material have a coating comprising a coating material with a thickness selected from the following list: less than 1 nm, less than 10 nm, less than 100 nm, or less than 1,000 nm. In some embodiments, the coating material has a thickness selected from the following list: less than 1 nm, less than 10 nm, or less than 100 nm.
[0192] In some embodiments, the ion exchange material and the coating material form one or more concentration gradients such that the chemical composition of coated ion exchange particles comprising the ion exchange material and the coating material ranges between two or more compositions. In some embodiments, the ion exchange material and the coating material form a concentration gradient within the coated ion exchange particles comprising the ion exchange material and the coating material that extends over a thickness selected from the following list: less than 1 nm, less than 10 nm, less than 100 nm, less than 1,000 nm, less than 10,000 nm, or less than 100,000 nm.
[0193] In some embodiments, coating thickness may be measured by any one or more of electron microscopy, optical microscopy, couloscopy, nanoindentation, atomic force microscopy, and X-ray fluorescence. In some embodiments, coating thickness may be inferred or extrapolated from data obtained according to an analytical method that indicates the bulk composition of the coated ion exchange particle, or the ion exchange material that further comprises the coating material. In some embodiments, coating thickness may be inferred by differential analysis of data obtained by analysis of ion exchange material that further comprises a coating material and data obtained by analysis ion exchange material that does not further comprise a coating material. In some embodiments, coating thickness may be inferred by differential analysis of data obtained by analysis of one or more coated ion exchange particles and data obtained by analysis of one or more uncoated ion exchange particles.
[0194] In some embodiments, the ion exchange material is synthesized by a method selected from the following list: hydrothermal, solvothermal, sol-gel, solid state, molten salt flux, ion exchange, microwave, ball milling, precipitation, or vapor deposition. In some embodiments, the ion exchange material is synthesized by a method selected from the following list: hydrothermal, solid state, or microwave.
[0195] In some embodiments, a coating material is deposited to form a coating by a method selected from the following list: chemical vapor deposition, atomic layer deposition, physical vapor deposition, hydrothermal, solvothermal, sol-gel, solid state, molten salt flux, ionWSGR Docket No. 50741-727.601exchange, microwave, wet impregnation, precipitation, titration, aging, ball milling, or combinations thereof. In some embodiments, the coating material is deposited to form a coating by a method selected from the following list: chemical vapor deposition, hydrothermal, titration, solvothermal, wet impregnation, sol-gel, precipitation, microwave, or combinations thereof.
[0196] In some embodiments, a coating material is deposited to form a coating with physical characteristics selected from the following list: crystalline, amorphous, full coverage, partial coverage, uniform, non-uniform, or combinations thereof.
[0197] In some embodiments, multiple coating materials are deposited to form multiple coatings on the ion exchange material in an arrangement selected from the following list: concentric, patchwork, or combinations thereof.
[0198] In some embodiments, the lithium selective sorbent composites comprise a porogen that is a salt that can be dissolved out of the lithium selective sorbent composites to form a network of pores within the lithium selective sorbent composites. In some embodiments, the lithium selective sorbent composites comprise a porogen that is a salt that can be dissolved out of the lithium selective sorbent composites using a solution selected from the following list: water, ethanol, isopropyl alcohol, a surfactant mixture, an acid, a base, or combinations thereof. In some embodiments, the lithium selective sorbent composites comprise a porogen that is a material that thermally decomposes to form a gas at high temperature such that the thermal decomposition of the filler material forms a network of pores within the lithium selective sorbent composite. In some embodiments, the lithium selective sorbent composites comprise a porogen that is a material that thermally decomposes to form a gas at high temperature wherein the gas is selected from the following list: water vapor, oxygen, nitrogen, chlorine, carbon dioxide, nitrogen oxides, organic vapors, or combinations thereof.
[0199] In some embodiments, the lithium selective sorbent composites are formed from dry powder. In some embodiments, the lithium selective sorbent composites are formed using a mechanical press, a pellet press, a tablet press, a pill press, a rotary press, or combinations thereof.
[0200] In some embodiments, the lithium selective sorbent composites are approximately spherical with an average diameter selected from the following list: less than 10 pm, less than 100 pm, less than 1 mm, less than 1 cm, or less than 10 cm. In some embodiments, the lithium selective sorbent composites are approximately spherical with an average diameter selected from the following list: less than 200 pm, less than 2 mm, or less than 20 mm.
[0201] In some embodiments, the lithium selective sorbent composites are tablet-shaped with a diameter of less than 1 mm, less than 2 mm, less than 4 mm, less than 8 mm, or less than 20 mmWSGR Docket No. 50741-727.601and with a height of less than 1 mm, less than 2 mm, less than 4 mm, less than 8 mm, or less than 20 mm.
[0202] In some embodiments, the lithium selective sorbent composites are embedded in a support structure, which can be a membrane, a spiral-wound membrane, a hollow fiber membrane, or a mesh. In some embodiments, the ion exchange materials are embedded on a support structure comprised of a polymer, a ceramic, or combinations thereof. In some embodiments, the lithium selective sorbent composites are loaded directly into an ion exchange column with no additional support structure.
[0203] In some embodiments, the liquid resource has a lithium concentration selected from the following list: less than 100,000 mg / L, less than 10,000 mg / L, less than 1,000 mg / L, less than 100 mg / L, less than 10 mg / L, or combinations thereof. In some embodiments, the liquid resource has a lithium concentration selected from the following list: less than 5,000 mg / L, less than 500 mg / L, less than 50 mg / L, or combinations thereof.
[0204] In some embodiments, the acid used for eluting lithium from the ion exchange material is selected from the following list: hydrochloric acid, sulfuric acid, phosphoric acid, hydrobromic acid, chloric acid, perchloric acid, nitric acid, formic acid, acetic acid, or combinations thereof. In some embodiments, the acid used for eluting lithium from the ion exchange material is selected from the following list: hydrochloric acid, sulfuric acid, nitric acid, or combinations thereof.
[0205] In some embodiments, the acid used for recovering lithium from the ion exchange material has an acid concentration selected from the following list: less than 0.1 M, less than 1.0 M, less than 5 M, less than 10 M, or combinations thereof. In some embodiments, the acid used for recovering lithium from the ion exchange material has an acid concentration of at least 0.05 M. In some embodiments, the acid used for recovering lithium from the ion exchange material has an acid concentration of at least 0.1 M. In some embodiments, the acid used for recovering lithium from the ion exchange material has an acid concentration of at least 1.0 M. In some embodiments, the acid used for recovering lithium from the ion exchange material has an acid concentration of at least 2.0 M. In some embodiments, the acid used for recovering lithium from the ion exchange material has an acid concentration of at least 5.0 M.
[0206] In some embodiments, the ion exchange material is utilized in an ion exchange process repeatedly over a number of cycles selected from the following list: greater than 10 cycles, greater than 30 cycles, greater than 100 cycles, greater than 300 cycles, or greater than 1,000 cycles. In some embodiments, the ion exchange material is utilized in an ion exchange process repeatedly over a number of cycles selected from the following list: greater than 50 cycles,WSGR Docket No. 50741-727.601greater than 100 cycles, or greater than 200 cycles. In some embodiments, the ion exchange material is utilized in an ion exchange process repeatedly over at least 500 cycles. In some embodiments, the ion exchange material is utilized in an ion exchange process repeatedly over at least 1,000 cycles. In some embodiments, the ion exchange material is utilized in an ion exchange process repeatedly over at least 2,000 cycles.
[0207] In some embodiments, a cycle comprises contacting a lithium-selective sorbent with a liquid resource to provide a lithiated lithium-selective sorbent and contacting the lithiated lithium-selective sorbent with an acidic solution (e.g., acid) to provide a synthetic lithium solution (e.g., lithium eluate). In some embodiments, the lithium-selective sorbent is used (e.g., a process for generating a synthetic lithium solution is conducted) for at least 10 cycles, at least 50 cycles, at least 100 cycles, at least 250 cycles, at least 500 cycles, at least 1000 cycles, at least 2000 cycles, at least 3000 cycles, at least 4000 cycles, at least 5000 cycles, at least 6000 cycles, at least 7000 cycles, at least 8000 cycles, at least 9000 cycles, or at least 10000 cycles.
[0208] In some embodiments, the synthetic lithium solution that is yielded from the ion exchange material is further processed into lithium chemicals, lithium compounds, or lithium raw materials using methods selected from the following list: solvent extraction, ion exchange, chemical precipitation, electrodialysis, electrowinning, evaporation with direct solar energy, evaporation with concentrated solar energy, evaporation with a heat transfer medium heated by concentrated solar energy, evaporation with heat from a geothermal brine, evaporation with heat from combustion, or combinations thereof.
[0209] In some embodiments, the synthetic lithium solution that is yielded from the ion exchange material is further processed into lithium chemicals selected from the following list: lithium chloride, lithium carbonate, lithium hydroxide, lithium metal, lithium metal oxide, lithium metal phosphate, lithium sulfide, or combinations thereof. In some embodiments, the synthetic lithium solution that is yielded from the ion exchange material is further processed into lithium chemicals that are solid, liquid, hydrated, or anhydrous.
[0210] In some embodiments, the lithium chemicals produced using the synthetic lithium solution are used in an industrial application selected from the following list: lithium batteries, metal alloys, glass, grease, or combinations thereof. In some embodiments, the lithium chemicals produced using the synthetic lithium solution derived from the ion exchange material are used in an industrial application selected from the following list: lithium batteries, metal alloys, glass, grease, or combinations thereof. In some embodiments, the lithium chemicals produced using the synthetic lithium solution derived from the coated ion exchange particles areWSGR Docket No. 50741-727.601used in an application selected from the following list: lithium batteries, lithium-ion batteries, lithium sulfur batteries, lithium solid-state batteries, and combinations thereof.
[0211] In some embodiments, the ion exchange materials are synthesized in a lithiated state, wherein a sublattice of the ion exchange material is fully or partially occupied by lithium. In some embodiments, the ion exchange materials are synthesized in a hydrogenated state, wherein a sublattice of the ion exchange material is fully or partially occupied by hydrogen.
[0212] For the purposes of this disclosure, the term lithium-selective sorbent comprises all lithium-selective ion exchange materials. Ion exchange materials that selectively absorb and release lithium ions are lithium-selective ion exchange materials. In some embodiments, lithium selective sorbent composites comprise a lithium-selective sorbent. In some embodiments, ion exchange particles comprise a lithium-selective sorbent. In some embodiments, lithium-selective sorbents comprise an inorganic material that selectively absorbs lithium over other ions. In some embodiments, a lithium selective sorbent is a crystalline lithium salt aluminate, a lithium aluminum intercalate, LiCl-2Al(OH)3, crystalline aluminum trihydroxide (Al(OH)3), gibbsite, beyerite, nordstrandite, alumina hydrate, bauxite, amorphous aluminum trihydroxide, activated alumina layered lithium-aluminum double hydroxides, LiAl2(OH)6Cl, combinations thereof, compounds thereof, or solid solutions thereof. In some embodiments, a mixed metal compound prepared according to any one of the methods for preparing a mixed metal compound described in the present disclosure is a lithium selective ion exchange material.
[0213] Lithium-selective ion exchange materials can be used in a method for lithium recovery from a liquid resource. Lithium-selective ion exchange materials can be used in a system for lithium recovery from a liquid resource. Lithium-selective ion exchange materials can be used in an ion exchange device. Lithium-selective ion exchange materials absorb lithium from a liquid resource while releasing hydrogen, and then elute lithium in an eluent while absorbing hydrogen from the eluent. This ion exchange process is optionally repeated to extract lithium from a liquid resource and yield a synthetic lithium solution. The synthetic lithium solution is optionally further processed into chemicals for the battery industry or other industries.
[0214] The performance parameters of lithium recovery by an ion exchange material are reflected in the ability of the ion exchange material to absorb lithium from a liquid resource in high quantity and in high purity over long periods time. When a given amount of an ion exchange material contacts a given amount of liquid resource, wash solution, eluent solution, or other process fluids, the effectiveness of selective lithium absorption, washing, lithium release / elution, or other treatment depends on effective contact of process fluids with the ion exchange material. In some embodiments, effective contact implies that a given amount of ionWSGR Docket No. 50741-727.601exchange material is contacted with the same amount of process fluid, and that the composition of said fluid is the same as that contacting the entirety of the ion exchange material. As such, in some embodiments, it is essential that devices for lithium recovery be configured in a manner such that the ion exchange material can make uniform contact with process fluids. In some embodiments, uniform contact implies that a liquid resource from which lithium is extracted uniformly contacts an ion exchange material which absorbs lithium while releasing protons.
[0215] Optimizing the performance parameters of lithium recovery is advantageous for lithium production from liquid resources using ion exchange processes that utilize one or more ion exchange materials. Disclosed herein are methods and systems for optimizing the performance parameters of lithium recovery using ion exchange materials that comprise lithium-selective sorbents by adjusting the concentration of lithium and pH of a liquid resource to be placed in contact with the ion exchange material. Adjusting the concentration of lithium in a liquid resource can yield a concentration-adjusted liquid resource according to some embodiments.
[0216] Adjusting the concentration of lithium in a liquid resource can result in the most optimal utilization of an ion exchange material utilized for lithium recovery, and helps ensure a prolonged lifetime of the ion exchange material. In some embodiments, the concentration of lithium in a liquid resource is increased to result in the most optimal utilization of an ion exchange material. In some embodiments, the concentration of lithium in a liquid resource is decreased to result in the most optimal utilization of an ion exchange material. In some embodiments, the pH of the liquid resource is adjusted in addition to the concentration of lithium in a liquid resource to result in the most optimal utilization of an ion exchange material.
[0217] In some embodiments, the most optimal utilization of an ion exchange material results in improved or optimized performance parameters for lithium recovery. In some embodiments, improved or optimized performance parameters comprise a longer useful lifetime of the ion exchange material used in the methods and systems described herein. In some embodiments, improved or optimized performance parameters comprise a higher lithium production rate for flow of the same amount of liquid resource across the ion exchange material used in the methods and systems described herein. In some embodiments, improved or optimized performance parameters comprise a higher lithium purity of the lithium provided by the ion exchange material used in the methods and systems described herein. In some embodiments, improved or optimized performance parameters comprise a greater quantity of lithium provided by a given quantity of ion exchange material over its useful lifetime when the ion exchange material is used according to the methods and systems described herein. In some embodiments, improved or optimized performance parameters comprise an increase in overall lithium recovery.WSGR Docket No. 50741-727.601
[0218] According to some embodiments of methods and systems for lithium recovery from a liquid resource, lithium is extracted from the liquid resources using inorganic lithium-selective sorbents that absorb lithium ions preferentially over other ions. In some embodiments, lithiumselective sorbents comprise lithium-selective ion exchange materials. As used herein, the term “lithium-selective ion-exchange material” refers to embodiments of “lithium-selective sorbent”. In some embodiments, the lithium-selective sorbent is a lithium-selective ion-exchange material. In some embodiments, the lithium-selective sorbent comprises lithium-selective ion-exchange particles. In some embodiments, the lithium selective sorbent comprises ion exchange particles. In some embodiments, the lithium-selective sorbent is an ion exchange material.
[0219] In some embodiments, lithium-selective sorbents include other inorganic materials that selectively absorb lithium over other ions. In some embodiments, lithium-selective sorbents selectively absorb lithium over other ions by processes that do not comprise ion exchange. In some embodiments, the lithium-selective sorbent is a crystalline lithium salt aluminate, a lithium aluminum intercalate, LiCl•2Al(OH)3, crystalline aluminum trihydroxide (Al(OH)3), gibbsite, beyerite, nordstrandite, alumina hydrate, bauxite, amorphous aluminum trihydroxide, activated alumina layered lithium-aluminum double hydroxides, LiAl2(OH)6Cl, combinations thereof, compounds thereof, or solid solutions thereof.
[0220] An aspect of the disclosure described herein is a device wherein the lithium-selective sorbent comprises an ion exchange material. An aspect of the disclosure described herein is a process wherein the lithium-selective sorbent comprises an ion-exchange material. An aspect of the disclosure described herein is a system wherein the lithium-selective sorbent comprises an ion-exchange material. An aspect of the disclosure described herein is a lithium-selective sorbent which extracts lithium from a liquid resource.
[0221] An aspect of the disclosure is a device, system, and associated process wherein the lithium-selective sorbent comprises a lithium aluminate intercalate. In some embodiments, the lithium aluminate intercalate mixed with a polymer material. In some embodiments, the polymer material comprises a chloro-polymer, a fluoro-polymer, a chloro-fluoro-polymer, a hydrophilic polymer, a hydrophobic polymer, co-polymers thereof, mixtures thereof, or combinations thereof. In some embodiments, the polymer material comprises a co-polymer, a block copolymer, a linear polymer, a branched polymer, a cross-linked polymer, a heat-treated polymer, a solution processed polymer, co-polymers thereof, mixtures thereof, or combinations thereof. In some embodiments, the polymer material comprises low density polyethylene, high density polyethylene, polypropylene, polyester, polytetrafluoroethylene (PTFE), types of polyamide, polyether ether ketone (PEEK), polysulfone, polyvinylidene fluoride (PVDF), poly (4-vinylWSGR Docket No. 50741-727.601pyridine-co-styrene) (PVPCS), polystyrene (PS), polybutadiene, acrylonitrile butadiene styrene (ABS), polyvinyl chloride (PVC), ethylene tetrafluoroethylene polymer (ETFE),poly (chlorotrifluoroethylene) (PCTFE), ethylene chlorotrifluoro ethylene (Halar), polyvinylfluoride (PVF), fluorinated ethylene-propylene (FEP), perfluorinated elastomer, chlorotrifluoroethylenevinylidene fluoride (FKM), perfluoropoly ether (PFPE), perfluoro-3,6-dioxa-4-methyl-7-octene-sulfonic acid (NAFION® (copolymer of perfluoro-3,6-dioxa-4-methyl-7-octene-sulfonic acid and tetrafluoroethylene)), polyethylene oxide, polyethylene glycol, sodium polyacrylate, polyethylene-block-poly(ethylene glycol), polyacrylonitrile (PAN), polychloroprene (neoprene), polyvinyl butyral (PVB), expanded polystyrene (EPS), polydivinylbenzene, co-polymers thereof, mixtures thereof, or combinations thereof. In some embodiments, the polymer material comprises polyvinylidene fluoride (PVDF), polyvinyl chloride (PVC), ethylene chlorotrifluoro ethylene (Halar), poly (4-vinyl pyridine-co-styrene) (PVPCS), polystyrene (PS), acrylonitrile butadiene styrene (ABS), expanded polystyrene (EPS), polyphenylene sulfide, sulfonated polymer, carboxylated polymer, other polymers, co-polymers thereof, mixtures thereof, or combinations thereof. In some embodiments, the polymer material is combined with the lithium aluminate intercalate particles by dry mixing, mixing in solvent, emulsion, extrusion, bubbling one solvent into another, casting, heating, evaporating, vacuum evaporation, spray drying, vapor deposition, chemical vapor deposition, microwaving, hydrothermal synthesis, polymerization, co-polymerization, cross-linking, irradiation, catalysis, foaming, other deposition methods, or combinations thereof. In some embodiments, the polymer material is combined with the lithium aluminate intercalate particles using a solvent comprising N-methyl-2-pyrrolidone, dimethyl sulfoxide, tetrahydrofuran, dimethylformamide, dimethylacetamide, methyl ethyl ketone, ethanol, acetone, other solvents, or combinations thereof. In a further aspect, a coating can be deposited onto the lithium aluminate intercalate particles using a solvent comprising N-methyl-2-pyrrolidone, dimethyl sulfoxide, tetrahydrofuran, dimethylformamide, dimethylacetamide, methyl ethyl ketone, ethanol, acetone, or combinations thereof.
[0222] In some embodiments, the lithium aluminate intercalate comprises particles that have an average diameter less than about 10 nm, less than about 100 nm, less than about 1,000 nm, less than about 10,000 nm, or less than about 100,000 nm. In some embodiments, the lithium aluminate intercalate comprises particles that have an average size less than about 100 nm, less than about 1,000 nm, or less than about 10,000 nm. In some embodiments, the lithium aluminate intercalate particles comprise secondary particles comprised of smaller primary particles wherein the smaller primary particles have an average diameter less than about 10 nm, less thanWSGR Docket No. 50741-727.601about 100 nm, less than about 1,000 nm, less than about 10,000 nm, or less than about 100,000 nm.
[0223] In a further aspect described herein, the lithium aluminate intercalate particles have an average diameter less than about 10 nm, less than about 100 nm, less than about 1,000 nm, less than about 10,000 nm, or less than about 100,000 nm. In a further aspect, the lithium aluminate intercalate particles have an average size less than about 100 nm, less than about 1,000 nm, or less than about 10,000 nm. In a further aspect, the lithium aluminate intercalate particles are optionally secondary particles comprised of smaller primary particles that have an average diameter less than about 10 nm, less than about 100 nm, less than about 1,000 nm, less than about 10,000 nm, or less than about 100,000 nm.Methods and systems for preparing a lithium selective sorbent composite
[0224] In one aspect, provided herein are lithium selective sorbent composites. Further provided herein are methods of preparing such lithium selective sorbent composites. In some embodiments, said methods comprise at least one of: 1) an extrusion process comprising passing the sorbent-binder semisolid through an extruder, and drying the sorbent-binder semisolid at a temperature of less than 500 Kelvin; 2) spray drying the sorbent-binder semisolid or the sorbentbinder slurry; and 3) spin flash drying the sorbent-binder semisolid or the sorbent-binder slurry. In some embodiments, said methods comprise: obtaining a sorbent-binder mixture; mixing the sorbent-binder mixture to form a sorbent-binder semisolid or a sorbent-binder slurry; and processing the sorbent-binder semisolid or the sorbent-binder slurry to afford a pre-calcined lithium selective sorbent composite, wherein processing comprises at least one of at least one of: 1) an extrusion process comprising passing the sorbent-binder semisolid through an extruder, and drying the sorbent-binder semisolid at a temperature of less than 500 Kelvin; 2) spray drying the sorbent-binder semisolid or the sorbent-binder slurry; and 3) spin flash drying the sorbentbinder semisolid or the sorbent-binder slurry. In some embodiments, the method comprises 1). In some embodiments, the method comprises 2). In some embodiments, the method comprises 3). In some embodiments, the method comprises 1) and 2). In some embodiments, the method comprises 2) and 3). In some embodiments, the method comprises 1) and 3). In some embodiments, the method comprises 1), 2), and 3).
[0225] Some embodiments of methods for preparing the lithium selective sorbent composite comprise an extrusion process, said extrusion process comprising passing the sorbent-binder semi solid through an extruder, and drying the sorbent-binder semisolid at a temperature of less than 500 Kelvin. In some embodiments, processing the sorbent-binder semisolid or the sorbent-WSGR Docket No. 50741-727.601binder slurry to afford a pre-calcine lithium selective sorbent composite comprises an extrusion process comprising passing the sorbent-binder semisolid through an extruder, and drying the sorbent-binder semisolid at a temperature of less than 500 Kelvin.
[0226] In some embodiments, the extruder is a cold feed extruder, a dome extruder, a basket extruder, a spheronizer, or a combination thereof. In some embodiments, the extruder provides an extrudate comprising the sorbent-binder semisolid. In some embodiments, the extruder is configured to provide an extrudate with a spherical shape, a cylindrical shape, a trilobe shape, a tetralobe shape, a tubular shape, a multi-channel monolith, or a combination thereof. In some embodiments, the extruder is a cold feed extruder. In some embodiments, the cold feed extruder is a single screw cold feed extruder or a coaxial twin screw cold feed extruder. In some embodiments, the cold feed extruder comprises liquid injection, a vacuum port, a barrel jacket for heating or cooling, or a combination thereof. In some embodiments, the cold feed extruder comprises variable screw flights for further mechanical mixing of the sorbent-binder semisolid.
[0227] In some embodiments, the extruder is configured to provide an extrudate with an average diameter of about 700 microns to about 5000 microns. In some embodiments, the extruder is configured to provide an extrudate with an average diameter of about 700 microns to about 1000 microns. In some embodiments, the extruder is configured to provide an extrudate with an average diameter of about 1000 microns to about 2000 microns. In some embodiments, the extruder is configured to provide an extrudate with an average diameter of about 2000 microns to about 3000 microns. In some embodiments, the extruder is configured to provide an extrudate with an average diameter of about 3000 microns to about 4000 microns. In some embodiments, the extruder is configured to provide an extrudate with an average diameter of about 4000 microns to about 5000 microns. In some embodiments, the extruder is configured to provide an extrudate with an average diameter of about 700 microns, about 800 microns, about 900 microns, about 1000 microns, about 1100 microns, about 1200 microns, about 1300 microns, about 1400 microns, about 1500 microns, about 1600 microns, about 1700 microns, about 1800 microns, about 1900 microns, about 2000 microns, about 2100 microns, about 2200 microns, about 2300 microns, about 2400 microns, about 2500 microns, about 2600 microns, about 2700 microns, about 2800 microns, about 2900 microns, about 3000 microns, about 3100 microns, about 3200 microns, about 3300 microns, about 3400 microns, about 3500 microns, about 3600 microns, about 3700 microns, about 3800 microns, about 3900 microns, about 4000 microns, about 4100 microns, about 4200 microns, about 4300 microns, about 4400 microns, about 4500 microns, about 4600 microns, about 4700 microns, about 4800 microns, about 4900 microns, or about 5000 microns. In some embodiments, the extruder is configured to operate at a lowWSGR Docket No. 50741-727.601pressure. Operating an extruder at a low pressure can provide extrudates with a smaller average particle diameter. In some embodiments, the extruder is configured to operate at a low pressure to provide an extrudate with an average particle diameter in the inclusive range of about 500 to about 1200 microns. In some embodiments, the extruder is configured to operate at a low pressure to provide an extrudate with an average particle diameter in the inclusive range of about 500 to about 750 microns. In some embodiments, the extruder is configured to operate at a low pressure to provide an extrudate with an average particle diameter in the inclusive range of about 750 to about 1000 microns. In some embodiments, the extruder is configured to operate at a low pressure to provide an extrudate with an average particle diameter in the inclusive range of about 1000 to about 1200 microns. In some embodiments, the dome extruder or the basket extruder is configured to provide an extrudate with a cylindrical shape and an average particle diameter in the inclusive range of about 500 to about 1200 microns. In some embodiments, the dome extruder or the basket extruder, or the spheronizer is configured to provide an extrudate with a cylindrical shape. In some embodiments, the spheronizer is configured to provide an extrudate with a spherical shape and an average particle diameter in the inclusive range of about 500 to about 1200 microns. In some embodiments, the spheronizer is configured to provide an extrudate with a spherical shape.
[0228] In some embodiments, drying the sorbent-binder semisolid at a temperature of less than 500 Kelvin is conducted by passing an extrudate comprising the sorbent-binder semisolid through a belt dryer, a fluidized belt dryer, a flash dryer, a spin mill flash dryer, a vacuum tray oven, or a combination thereof. In some embodiments, drying the sorbent-binder semisolid at a temperature of less than 500 Kelvin is conducted in the inclusive range of about 30 to about 150 degrees Celsius. In some embodiments, drying the sorbent-binder semisolid at a temperature of less than 500 Kelvin is conducted in the inclusive range of about 30 to about 130 degrees Celsius. In some embodiments, drying the sorbent-binder semisolid at a temperature of less than 500 Kelvin is conducted in the inclusive range of about 50 to about 150 degrees Celsius. In some embodiments, drying the sorbent-binder semisolid at a temperature of less than 500 Kelvin is conducted at about 30 degrees Celsius, about 40 degrees Celsius, about 50 degrees Celsius, about 60 degrees Celsius, about 70 degrees Celsius, about 80 degrees Celsius, about 90 degrees Celsius, about 100 degrees Celsius, about 110 degrees Celsius, about 120 degrees Celsius, about 130 degrees Celsius, about 140 degrees Celsius, or about 150 degrees Celsius. In some embodiments, drying the sorbent-binder semisolid at a temperature of less than 500 Kelvin is conducted for a residence time. In some embodiments, the residence time is the quantity of time the extrudate is exposed to an environment maintained at the temperature of less than 500WSGR Docket No. 50741-727.601Kelvin. In some embodiments, the residence time is about 10 to about 120 minutes. In some embodiments, the residence time is about 10 to about 30 minutes. In some embodiments, the residence time is about 30 to about 60 minutes. In some embodiments, the residence time is about 60 to about 120 minutes. In some embodiments, the residence time is about 60 to about 90 minutes. In some embodiments, the residence time is about 90 to about 120 minutes. In some embodiments, the residence time is about 10 minutes, about 20 minutes, about 30 minutes, about 40 minutes, about 50 minutes, about 60 minutes, about 70 minutes, about 80 minutes, about 90 minutes, about 100 minutes, about 110 minutes, about 120 minutes, about 130 minutes, about 140 minutes, or about 150 minutes.
[0229] Some embodiments of methods for preparing the lithium selective sorbent composite comprise spray drying the sorbent-binder semisolid or the sorbent-binder slurry. In some embodiments, processing the sorbent-binder semisolid or the sorbent-binder slurry to afford a pre-calcined lithium selective sorbent composite comprises spray drying the sorbent-binder semisolid or the sorbent-binder slurry. In some embodiments, spray drying the sorbent-binder semi solid or the sorbent-binder slurry provides a pre-calcined lithium selective sorbent composite that has a d97 of about 25 microns or less. In some embodiments, spray drying the sorbent-binder semisolid or the sorbent-binder slurry provides a pre-calcined lithium selective sorbent composite that has a d97 of about 25 microns, about 20 microns, about 18 microns, about 15 microns, about 12 microns, about 10 microns, about 8 microns, about 5 microns, about 2 microns, about 1 micron, or less than about 1 micron. The parameter d97 describes the maximum diameter of at least 97% of the pre-calcined lithium selective sorbent composite. In some embodiments, the spray dryer is configured to operate at an outlet temperature of about 125 to about 150 degrees Celsius. In some embodiments, the spray dryer is configured to operate at an outlet temperature of about 50 degrees Celsius, about 60 degrees Celsius, about 70 degrees Celsius, about 80 degrees Celsius, about 90 degrees Celsius, about 100 degrees Celsius, about 110 degrees Celsius, about 120 degrees Celsius, about 130 degrees Celsius, about 140 degrees Celsius, or about 150 degrees Celsius.
[0230] Some embodiments of methods for preparing the lithium selective sorbent composite comprise spin flash drying the sorbent-binder semisolid or the sorbent-binder slurry. In some embodiments, processing the sorbent-binder semisolid or the sorbent-binder slurry to afford a pre-calcined lithium selective sorbent composite comprises spin flash drying the sorbent-binder semisolid or the sorbent-binder slurry. In some embodiments, spin flash drying the sorbentbinder semi solid or the sorbent-binder slurry provides a pre-calcined lithium selective sorbent composite that has a d97 of about 150 microns or less. In some embodiments, spin flash dryingWSGR Docket No. 50741-727.601the sorbent-binder semisolid or the sorbent-binder slurry provides a pre-calcined lithium selective sorbent composite that has a d97 of about 150 microns, about 140 microns, about 130 microns, about 120 microns, about 110 microns, about 100 microns, about 90 microns, about 80 microns, about 70 microns, about 60 microns, about 50 microns, about 40 microns, about 30 microns, about 20 microns, about 10 microns, or less than about 10 microns. The parameter d97 describes the maximum diameter of at least 97% of the pre-calcined lithium selective sorbent composite. In some embodiments, the spin flash dryer utilizes hot air to dry and convey the sorbent-binder semisolid or the sorbent-binder slurry upwards towards a classifier mill. In some embodiments, the classifier mill is configured to control the particle size distribution of the precalcined lithium selective sorbent composite. In some embodiments, the spin flash dryer is configured to operate at an outlet temperature of about 50 to about 150 degrees Celsius. In some embodiments, the spin flash dryer is configured to operate at an outlet temperature of about 50 to about 75 degrees Celsius. In some embodiments, the spin flash dryer is configured to operate at an outlet temperature of about 75 to about 100 degrees Celsius. In some embodiments, the spin flash dryer is configured to operate at an outlet temperature of about 100 to about 125 degrees Celsius. In some embodiments, the spin flash dryer is configured to operate at an outlet temperature of about 125 to about 150 degrees Celsius. In some embodiments, the spin flash dryer is configured to operate at an outlet temperature of about 50 degrees Celsius, about 60 degrees Celsius, about 70 degrees Celsius, about 80 degrees Celsius, about 90 degrees Celsius, about 100 degrees Celsius, about 110 degrees Celsius, about 120 degrees Celsius, about 130 degrees Celsius, about 140 degrees Celsius, or about 150 degrees Celsius.
[0231] In some embodiments, the pre-calcined lithium selective sorbent composite is prepared without milling. In some embodiments, the pre-calcined lithium selective sorbent composite is prepared without milling by feeding the sorbent-binder semisolid or the sorbent-binder slurry into a flash dryer. In some embodiments, the flash dryer utilizes hot air to dry and convey the sorbent-binder semisolid or the sorbent-binder slurry upwards to a dust collection system. In some embodiments, the flash dryer is configured to operate at an outlet temperature of about 125 to about 150 degrees Celsius. In some embodiments, the flash dryer is configured to operate at an outlet temperature of about 50 degrees Celsius, about 60 degrees Celsius, about 70 degrees Celsius, about 80 degrees Celsius, about 90 degrees Celsius, about 100 degrees Celsius, about 110 degrees Celsius, about 120 degrees Celsius, about 130 degrees Celsius, about 140 degrees Celsius, or about 150 degrees Celsius.
[0232] In some embodiments, the pre-calcined lithium selective sorbent composite is collected via dust collection prior to a sizing process or a calcination process. In some embodiments, theWSGR Docket No. 50741-727.601pre-calcined lithium selective sorbent composite is subjected to a calcination process, a sizing process, or a combination thereof. In some embodiments, the sizing process precedes the calcination process. In some embodiments, the calcination process precedes the sizing process. In some embodiments, a first sizing process and a second sizing process are conducted, wherein the first sizing process and the second sizing process are independently selected and configured, and wherein the first sizing process is conducted before a calcination process and the second sizing process is conducted after the calcination process. The first sizing process and the second sizing process can independently comprise, but are not limited to, any embodiment of a sizing process described in the present disclosure.Lithium Selective Sorbent Composites
[0233] In one aspect, the present disclosure provides lithium selective sorbent composites. In another aspect, the present disclosure provides methods for preparing said lithium selective sorbent composites. In a further aspect, the present disclosure provides methods for using said lithium selective sorbent composites in methods for lithium extraction, such as lithium extraction from a liquid resource. The foregoing description, provides a variety of non-limiting embodiments, features, and considerations for providing a lithium selective sorbent composite from a lithium selective sorbent.
[0234] In some embodiments, the lithium selective sorbent composites comprise a mixed metal compound produced by the methods and systems described herein. In some embodiments, the lithium selective sorbent composites comprise a lithium selective sorbent. In some embodiments, the lithium selective sorbent is an ion exchange material. In some embodiments, the lithium selective sorbent composites of the disclosure serve as an ion exchange material in a method, device, or system for lithium extraction. Accordingly, the lithium selective sorbent composites of the present disclosure can be used in conjunction with at least the methods for lithium extraction, the devices for lithium extraction, and the systems for lithium extraction described throughout the present disclosure. Upon consideration of the disclosure as a whole, it will be appreciated that the lithium selective sorbent composites provided herein can be used in a variety of adaptations of and alternatives to the methods for lithium extraction, the devices for lithium extraction, and the systems for lithium extraction described throughout the present disclosure.
[0235] In one aspect, provided herein are lithium selective sorbent composites. Further provided herein are methods of preparing such lithium selective sorbent composites, wherein saidWSGR Docket No. 50741-727.601methods can comprise obtaining a sorbent-binder mixture and mixing the sorbent-binder mixture to form a sorbent-binder semisolid or a sorbent-binder slurry.
[0236] For the purposes of this disclosure, the binder may be equivalently referred to as a “structural matrix material” or “matrix material”. As such, additional embodiments of the lithium selective sorbent are contemplated in the section “Beads Comprising a Lithium Selective sorbent and a Structural Matrix Material.”
[0237] In some embodiments, the sorbent-binder mixture comprises a lithium selective sorbent. The lithium selective sorbent can be any lithium selective sorbent described in any section of the present disclosure. For the purposes of the present disclosure, a lithium selective sorbent is an active material according to some embodiments. In some embodiments, the lithium selective sorbent is an ion exchange material. In some embodiments, the lithium selective sorbent is a lithium-selective ion exchange material.
[0238] In some embodiments, the lithium selective sorbent is a lithium titanium oxide. In some embodiments, the lithium selective sorbent is provided by contacting a lithium titanium oxide to an acidic solution, thereby exchanging, partially or wholly, lithium ions from the lithium titanium oxide with hydrogen ions from the acidic solution. In some embodiments, the lithium selective sorbent is a lithium manganese oxide. In some embodiments, the lithium selective sorbent is provided by contacting a lithium manganese oxide to an acidic solution, thereby exchanging, partially or wholly, lithium ions from the lithium manganese oxide with hydrogen ions from the acidic solution. In some embodiments, the lithium selective sorbent comprises Li4Mn5O12, Li4Ti5O12, Li2TiC>3, Li2MnO3, Li2SnO3, LiMn2O4, Li1.6Mn1.6O4, LiAlO2, LiCuO2, LiTiO2, Li4TiO4, Li7Ti11O24, Li3VO4, Li2Si3O7, LiFePO4, LiMnPO4, Li2CuP2O7, Al(OH)3, a solid solution thereof, or a combination thereof.
[0239] The lithium selective sorbent can be further characterized by its average particle size or particle size distribution. In some embodiments, the lithium selective sorbent used in preparing the lithium selective sorbent composites has a characteristic average particle size or particle size distribution. As such, the lithium selective sorbent used to prepare the sorbent-binder mixture can be in the form of particles, such as ion exchange particles. In some embodiments, the D50 of the lithium selective sorbent is within the inclusive range of about 1 to about 100 microns. In some embodiments, the D50 of the lithium selective sorbent is about 1 microns. In some embodiments, the D50 of the lithium selective sorbent is about 5 microns. In some embodiments, the D50 of the lithium selective sorbent is about 10 microns. In some embodiments, the D50 of the lithium selective sorbent is about 15 microns. In some embodiments, the D50 of the lithium selective sorbent is about 20 microns. In someWSGR Docket No. 50741-727.601embodiments, the D50 of the lithium selective sorbent is about 30 microns. In some embodiments, the D50 of the lithium selective sorbent is about 40 microns. In some embodiments, the D50 of the lithium selective sorbent is about 60 microns. In some embodiments, the D50 of the lithium selective sorbent is about 70 microns. In some embodiments, the D50 of the lithium selective sorbent is about 80 microns. In some embodiments, the D50 of the lithium selective sorbent is about 90 microns. In some embodiments, the D50 of the lithium selective sorbent is about 100 microns. The parameter D50 specifies that 50% of the particles are larger than the specified value, and 50% of the particles are smaller than the specified value.
[0240] In some embodiments, the sorbent-binder mixture comprises a binder. In some embodiments, the sorbent-binder mixture comprises a binder and a lithium selective sorbent. In some embodiments, the sorbent-binder mixture comprises multiple binders. In some embodiments, the sorbent-binder mixture comprises two binders. In some embodiments, the sorbent-binder mixture comprises three binders. In some embodiments, the sorbent-binder mixture comprises four, five, or more than five binders. In some embodiments, the sorbentbinder mixture comprises a lithium selective sorbent and at least one binder. When the sorbentbinder mixture comprises more than one binder, each of said binders can be selected independently. It shall be understood that, unless specified otherwise, the embodiments of a binder described herein are each contemplated for use both with additional binders and without additional binders.
[0241] In some embodiments, the sorbent-binder mixture is further characterized by the mass ratio of the lithium selective sorbent to the binder (e.g., one or more binders) in the sorbentbinder mixture. In some embodiments, the mass ratio of the lithium selective sorbent to the binder is about 1:10,000 to about 10,000:1. In some embodiments, the mass ratio of the lithium selective sorbent to the binder is about 1: 1,000 to about 1,000: 1. In some embodiments, the mass ratio of the lithium selective sorbent to the binder is about 1: 100 to about 100: 1. In some embodiments, the mass ratio of the lithium selective sorbent to the binder is about 1: 100 to about 10: 1. In some embodiments, the mass ratio of the lithium selective sorbent to the binder is about 1: 100 to about 1: 1. In some embodiments, the mass ratio of the lithium selective sorbent to the binder is about 1:100, about 1:90, about 1:80, about 1:70, about 1:60, about 1:50, about 1:45, about 1:40, about 1:35, about 1:30, about 1:25, about 1:20, about 1:15, about 1:10, about 1:9, about 1:8, about 1:7, about 1:6, about 1:5, about 1:4, about 1:3, about 1:2, about 1:1.8, about 1:1.6, about 1:1.4, about 1:1.2, about 1: 1.1, or about 1:1.WSGR Docket No. 50741-727.601
[0242] In some embodiments, the sorbent-binder mixture comprises one or more binders. When the sorbent-binder mixture comprises more than one binder, the sorbent-binder mixture can be further characterized by the mass ratios of one binder to another binder. In some embodiments, the sorbent-binder mixture comprises two binders (e.g., a first binder and a second binder). In some embodiments, the mass ratio of the first binder to the second binder is about 1: 100 to about 1:1. In some embodiments, the sorbent-binder mixture comprises three binders (e.g., a first binder, a second binder, and a third binder). In some embodiments, the mass ratio of the first binder to the second binder can be about 1: 100 to about 1:1, and the mass ratio of the first binder to the third binder can be about 1: 100 to about 1: 1. In some embodiments, the mass ratio of the first binder to the second binder can be about 1: 100 to about 1:1, and the mass ratio of the second binder to the third binder can be about 1: 100 to about 1: 1. In some embodiments, the sorbent-binder mixture comprises more than three binders.
[0243] In some embodiments, the binder comprises silica or a silica precursor. In some embodiments, the binder comprises silica. In some embodiments, the silica is porous, amorphous, or both. In some embodiments, the binder comprises a silica precursor. In some embodiments, a silica precursor is a chemical compound or material comprising silicon that can be modified to provide silica. For example, a silica precursor can be modified by heating to provide silica. For example, a silica precursor can be modified by chemical decomposition to provide silica. For example, a silica precursor can be modified by contacting the silica precursor to one or more chemical reagents to provide silica. For example, a silica precursor can be modified by hydrolysis, condensation, or a combination thereof to provide silica. In some embodiments, the silica precursor comprises colloidal silica, a tetraalkyl orthosilicate, fumed silica, a silicate and / or its dissolved water glasses, a natural source of silica, or a combination thereof.
[0244] In some embodiments, the silica precursor comprises colloidal silica. In some embodiments, the colloidal silica comprises siloxide groups (Si-O‘ groups) and counterions. In some embodiments, the colloidal silica comprises counterions selected from sodium, ammonium, hydrogen, and a combination thereof. The colloidal silica can be further characterized by its average particle size or particle size distribution. In some embodiments, the colloidal silica used in preparing the lithium selective sorbent composites has a characteristic average particle size or particle size distribution. In some embodiments, the average particle size of the colloidal silica is within the inclusive range of about 5 to about 100 nm. In some embodiments, the average particle size of the colloidal silica is within the inclusive range of about 5 to about 25 nm. In some embodiments, the average particle size of the colloidal silica isWSGR Docket No. 50741-727.601within the inclusive range of about 5 to about 50 nm. In some embodiments, the average particle size of the colloidal silica is within the inclusive range of about 25 to about 100 nm. In some embodiments, the average particle size of the colloidal silica is within the inclusive range of about 50 to about 100 nm. The colloidal silica can be further characterized by its surface area. In some embodiments, the colloidal silica used in preparing the lithium selective sorbent composites has a characteristic surface area. In some embodiments, the colloidal silica has a surface area within the inclusive range of about 100 to about 350 m2 / g. In some embodiments, the colloidal silica has a surface area within the inclusive range of about 100 to about 200 m2 / g. In some embodiments, the colloidal silica has a surface area within the inclusive range of about 200 to about 350 m2 / g. In some embodiments, the colloidal silica has a surface area within the inclusive range of about 300 to about 350 m2 / g.
[0245] In some embodiments, the binder comprises alumina or an alumina precursor. In some embodiments, the binder comprises alumina. In some embodiments, the alumina is porous, amorphous, or both. In some embodiments, the binder comprises an alumina precursor. In some embodiments, an alumina precursor is a chemical compound or material comprising aluminum that can be modified to provide alumina. For example, an alumina precursor can be modified by heating to provide alumina. For example, an alumina precursor can be modified by chemical decomposition to provide alumina. For example, an alumina precursor can be modified by contacting the alumina precursor to one or more chemical reagents to provide alumina. For example, an alumina precursor can be modified by hydrolysis, condensation, or a combination thereof to provide alumina. In some embodiments, the alumina precursor comprises boehmite, pseudoboehmite, gibbsite, bayerite, aluminum chloride, aluminum hydroxide, or a combination thereof.
[0246] In some embodiments, the alumina precursor comprises boehmite. In some embodiments, boehmite is an aluminum oxide hydroxide mineral with the chemical formula AlO2H. In some embodiments, boehmite is a component of bauxite ores. In some embodiments, boehmite is crystalline. In some embodiments, boehmite crystallizes in the orthorhombic space group Amam. Following calcination, the boehmite can be further characterized by its surface area. In some embodiments, upon calcination the boehmite has a surface area within the inclusive range of about 100 to about 450 m2 / g. In some embodiments, upon calcination the boehmite has a surface area within the inclusive range of about 100 to about 200 m2 / g. In some embodiments, upon calcination the boehmite has a surface area within the inclusive range of about 200 to about 300 m2 / g. In some embodiments, upon calcination the boehmite has a surface area within the inclusive range of about 300 to about 450 m2 / g.WSGR Docket No. 50741-727.601
[0247] In some embodiments, the alumina precursor comprises pseudoboehmite. In some embodiments, pseudoboehmite is an aluminum oxide hydroxide mineral with the chemical formula AlO2H. In some embodiments, pseudoboehmite is comprises finely crystalline boehmite. In some embodiments, the water content of pseudoboehmite is higher than the water content of boehmite. Following calcination, the pseudoboehmite can be further characterized by its surface area. In some embodiments, upon calcination the pseudoboehmite has a surface area within the inclusive range of about 100 to about 450 m2 / g. In some embodiments, upon calcination the pseudoboehmite has a surface area within the inclusive range of about 100 to about 200 m2 / g. In some embodiments, upon calcination the pseudoboehmite has a surface area within the inclusive range of about 200 to about 300 m2 / g. In some embodiments, upon calcination the pseudoboehmite has a surface area within the inclusive range of about 300 to about 450 m2 / g.
[0248] In some embodiments, the alumina precursor comprises gibbsite. In some embodiments, gibbsite is an aluminum hydroxide mineral with the chemical formula Al(OH)3. In some embodiments, the gibbsite is bayerite. In some embodiments, bayerite is gibbsite with a monoclinic crystal structure. In some embodiments, gibbsite has a crystal structure that is monoclinic, triclinic, or a combination thereof. Following calcination, the bayerite can be further characterized by its surface area. In some embodiments, upon calcination the bayerite has a surface area within the inclusive range of about 100 to about 450 m2 / g. In some embodiments, upon calcination the bayerite has a surface area within the inclusive range of about 100 to about 200 m2 / g. In some embodiments, upon calcination the bayerite has a surface area within the inclusive range of about 200 to about 300 m2 / g. In some embodiments, upon calcination the bayerite has a surface area within the inclusive range of about 300 to about 450 m2 / g.
[0249] In some embodiments, the alumina precursor comprises aluminum chloride. In some embodiments, the alumina precursor comprises aluminum hydroxide.
[0250] In some embodiments, the binder comprises a metal oxide or a metal oxide precursor. In some embodiments, the metal oxide is yttria (Y2O3), zirconia (ZrO2), titania (TiO2), or a combination thereof. In some embodiments, the metal oxide precursor is an yttria, a zirconia precursor, a titania precursor, or a combination thereof.
[0251] In some embodiments, the binder comprises a mixed metal oxide or a mixed metal oxide precursor. In some embodiments, the mixed metal oxide is a silicon aluminum oxide. In some embodiments, the mixed metal oxide precursor is a silicon aluminum oxide precursor. In some embodiments, the silicon aluminum oxide precursor comprises silica, alumina, a silica precursor, an alumina precursor, or a combination thereof. In some embodiments, the mixed metal oxide isWSGR Docket No. 50741-727.601porous, amorphous, or both. In some embodiments, the silicon aluminum oxide precursor comprises amorphous silica alumina, bentonite, callanite, a natural zeolite, a synthetic zeolite, or a combination thereof.Beads Comprising a Lithium Selective Sorbent and a Structural Matrix Material
[0252] In some embodiments, lithium selective sorbent composites are formed into a bead, said bead comprising an ion exchange material. Therefore, embodiments described herein for “ion exchange beads” should be understood to apply to any embodiments for “ion exchange material”, or for any material composition comprising an ion exchange material, including but not limited to coated ion exchange material(s), beads comprising coated ion exchange material(s), ion exchange materials embedded in a structural support, ion exchange materials embedded in a matrix, composites comprising ion exchange material(s), lithium selective sorbent composites - wherein the lithium selective sorbent comprises an ion exchange material, or combinations thereof.
[0253] In some embodiments, the ion exchange beads are formed by mixing of ion exchange material, a structural matrix material, and a filler material. In some embodiments, the ion exchange beads are formed by mixing of ion exchange material and a structural matrix material. In some embodiments, said matrix material is referred to as a structural support. In some embodiments, the ion exchange beads are formed by mixing of ion exchange material and a structural matrix material. In some embodiments, the components of an ion exchange bead combined to form a physical mixture or a composite. In some embodiments wherein an ion exchange bead comprises a filler material, the filler material can be removed therefrom to form network of pores therein and yield a porous ion exchange bead. The filler material is dispersed in the bead in such a way to leave behind a pore structure that enables transport of lithium and hydrogen with fast kinetics. In some embodiments, an ion exchange bead comprises one or more ion exchange materials, one or more structural matrix materials, and one or more filler materials.
[0254] In some embodiments, the mixed metal compound is embedded in, adhered to, or otherwise supported by a structural to form the porous structure.
[0255] In some embodiments, the structural matrix material is selected from the following list: a polymer, an oxide, a phosphate, or combinations thereof. In some embodiments, a structural matrix material is selected from the following list: polyvinyl fluoride, polyvinylidene difluoride, polyvinyl chloride, polyvinylidene dichloride, polyethylene, polypropylene, polyphenylene sulfide, polytetrafluoroethylene, polytetrafluoroethylene, sulfonated polytetrafluoroethylene, polystyrene, polydivinylbenzene, polybutadiene, sulfonated polymer, carboxylated polymer,WSGR Docket No. 50741-727.601Nafion, copolymers thereof, and combinations thereof. In some embodiments, a structural matrix material is selected from the following list: polyvinylidene difluoride, polyvinyl chloride, sulfonated polytetrafluoroethylene, polystyrene, polydivinylbenzene, copolymers thereof, or combinations thereof. In some embodiments, a structural matrix material is selected from the following list: titanium dioxide, zirconium dioxide, silicon dioxide, solid solutions thereof, or combinations thereof. In some embodiments, the structural matrix material is selected for its thermal durability, acid resistance, and / or other chemical resistance.
[0256] In some embodiments, the porous ion exchange bead is formed by a process comprising mixing ion exchange particles, structural matrix material, and filler material together at once. In some embodiments, the porous ion exchange bead is formed by a process comprising mixing the ion exchange particles and the structural matrix material, and then mixing the resulting mixture with the filler material. In some embodiments, the porous ion exchange bead is formed by a process comprising mixing the ion exchange particles and the filler material, and then mixing the resulting mixture with the structural matrix material. In some embodiments, the porous ion exchange bead is formed by a process comprising mixing the structural matrix material and the filler material, and then mixing the resulting mixture with the ion exchange particles.
[0257] In some embodiments, the porous ion exchange bead is formed by a process comprising mixing the ion exchange particles, the structural matrix material, and / or the filler material with a solvent that dissolves one or more of the components of the mixture. In some embodiments, the porous ion exchange bead is formed by a process comprising mixing the ion exchange particles, the structural matrix material, and / or the filler material as dry powders in a mixer or ball mill. In some embodiments, the porous ion exchange bead is formed by a process comprising mixing the ion exchange particles, the structural matrix material, and / or the filler material in a spray drier.
[0258] In some embodiments, the structural matrix material is a polymer that is dissolved in a solvent and subsequently mixed with the ion exchange particles and / or filler material using a solvent from the following list: N-methyl-2-pyrrolidone, dimethyl sulfoxide, tetrahydrofuran, dimethylformamide, dimethylacetamide, methyl ethyl ketone, or combinations thereof. In some embodiments, the filler material is a salt that is dissolved in a solvent and subsequently mixed with the ion exchange particles and / or structural matrix material using a solvent from the following list: water, ethanol, isopropyl alcohol, acetone, or combinations thereof.
[0259] In some embodiments, the ion exchange beads comprise a filler material that is a salt that can be dissolved out of the ion exchange bead to form a network of pores within the ion exchange bead. In some embodiments, the ion exchange beads comprise a filler material that is a salt that can be dissolved out of the ion exchange bead using a solution selected from theWSGR Docket No. 50741-727.601following list: water, ethanol, isopropyl alcohol, a surfactant mixture, an acid, a base, or combinations thereof. In some embodiments, the ion exchange beads comprise a filler material that is a material that thermally decomposes to form a gas at high temperature such that the thermal decomposition of the filler material forms a network of pores within the ion exchange bead. In some embodiments, the ion exchange beads comprise a filler material that is a material that thermally decomposes to form a gas at high temperature wherein the gas is selected from the following list: water vapor, oxygen, nitrogen, chlorine, carbon dioxide, nitrogen oxides, organic vapors, or combinations thereof.
[0260] In some embodiments, the mixed ion exchange beads have a pore size distribution with a characteristic D50 value. The parameter D50 specifies that 50% of the pores are larger than the specified value, and 50% of the pores are smaller than the specified value. In some embodiments, the D50 value is about 1 mm. In some embodiments, the D50 value is about 2 mm. In some embodiments, the D50 value is from about 0.4 mm to about 3 mm. In some embodiments, the D50 value is from about 1 mm to about 10 mm. In some embodiments, the D50 value is about 0.4 mm, about 1 mm, about 2 mm, about 3 mm, about 4 mm, about 5 mm, about 6 mm, about 7 mm, about 8 mm, about 9 mm, or about 10 mm. In some embodiments, the D50 value is from about 70 microns to about 700 microns. In some embodiments, the D50 value is from about 10 microns to about 70 microns. In some embodiments, the D50 value is from about 1 microns to about 10 microns. In some embodiments, the D50 value is from about 0.1 microns to about 1 microns.
[0261] In some embodiments, a coating material used to form a coating on the lithium selective sorbent. In some embodiments, a coating material used to form a coating on an ion exchange material or on ion exchange particles that comprise an ion exchange material is selected from the following list: a carbide, a nitride, an oxide, a phosphate, a fluoride, a polymer, carbon, a carbonaceous material, or combinations thereof. In some embodiments, the coating material comprises an oxide different from the oxide of the ion exchange material. In some embodiments, a coating material is selected from the following list: TiCh, ZrCh, MoO?, SnCh, bt^Os, Ta20s, SiC>2, Li2TiO3, Li2ZrOs, Li2SiOs, Li2MnO3, Li2MoOs, LiNbCh, LiTaCh, AIPO4, LaPC>4, ZrP2O?, MOP2O7, MO2P3O12, BaSO4, AIF3, SiC, TiC, ZrC, SisN4, ZrN, BN, carbon, graphitic carbon, amorphous carbon, hard carbon, diamond-like carbon, solid solutions thereof, or combinations thereof. In some embodiments, a coating material is selected from the following list: TiCh, ZrCh, MoO2, SiC>2, Li2TiC>3, Li2ZrO3, Li2SiO3, Li2MnO3, LiNbCh, AIF3, SiC, SisN4, graphitic carbon, amorphous carbon, diamond-like carbon, or combinations thereof.WSGR Docket No. 50741-727.601
[0262] In some embodiments, the ion exchange material or the ion exchange particles comprising an ion exchange material have a coating comprising a coating material with a thickness selected from the following list: less than 1 nm, less than 10 nm, less than 100 nm, or less than 1,000 nm. In some embodiments, the coating material has a thickness selected from the following list: less than 1 nm, less than 10 nm, or less than 100 nm.
[0263] In some embodiments, the ion exchange material and the coating material form one or more concentration gradients such that the chemical composition of coated ion exchange particles comprising the ion exchange material and the coating material ranges between two or more compositions. In some embodiments, the ion exchange material and the coating material form a concentration gradient within the coated ion exchange particles comprising the ion exchange material and the coating material that extends over a thickness selected from the following list: less than 1 nm, less than 10 nm, less than 100 nm, less than 1,000 nm, less than 10,000 nm, or less than 100,000 nm.
[0264] In some embodiments, coating thickness may be measured by any one or more of electron microscopy, optical microscopy, couloscopy, nanoindentation, atomic force microscopy, and X-ray fluorescence. In some embodiments, coating thickness may be inferred or extrapolated from data obtained according to an analytical method that indicates the bulk composition of the coated ion exchange particle, or the ion exchange material that further comprises the coating material. In some embodiments, coating thickness may be inferred by differential analysis of data obtained by analysis of ion exchange material that further comprises a coating material and data obtained by analysis ion exchange material that does not further comprise a coating material. In some embodiments, coating thickness may be inferred by differential analysis of data obtained by analysis of one or more coated ion exchange particles and data obtained by analysis of one or more uncoated ion exchange particles.
[0265] In some embodiments, the ion exchange material is synthesized by a method selected from the following list: hydrothermal, solvothermal, sol-gel, solid state, molten salt flux, ion exchange, microwave, ball milling, precipitation, or vapor deposition. In some embodiments, the ion exchange material is synthesized by a method selected from the following list: hydrothermal, solid state, or microwave.
[0266] In some embodiments, a coating material is deposited to form a coating by a method selected from the following list: chemical vapor deposition, atomic layer deposition, physical vapor deposition, hydrothermal, solvothermal, sol-gel, solid state, molten salt flux, ion exchange, microwave, wet impregnation, precipitation, titration, aging, ball milling, or combinations thereof. In some embodiments, the coating material is deposited to form a coatingWSGR Docket No. 50741-727.601by a method selected from the following list: chemical vapor deposition, hydrothermal, titration, solvothermal, wet impregnation, sol-gel, precipitation, microwave, or combinations thereof.
[0267] In some embodiments, a coating material is deposited to form a coating with physical characteristics selected from the following list: crystalline, amorphous, full coverage, partial coverage, uniform, non-uniform, or combinations thereof.
[0268] In some embodiments, multiple coating materials are deposited to form multiple coatings on the ion exchange material in an arrangement selected from the following list: concentric, patchwork, or combinations thereof.Process of extracting lithium from a liquid resource
[0269] In one aspect described herein, is a process for lithium extraction from a liquid resource comprising treating an ion exchange material alternately with acid, brine, and optionally other solutions, in a configuration where the beads move in the net opposite direction to the acid, brine, and optionally other solutions, thereby producing a lithium-enriched solution from the liquid resource. In one embodiment, the process comprises: (a) treating the ion exchange material with acid under conditions suitable to absorb hydrogen to generate hydrogen-enriched beads and release lithium to generate a lithium-enriched solution; (b) optionally, washing the hydrogen-enriched ion exchange material with water to generate a hydrogen-enriched ion exchange material substantially free of residual acid; (c) treating the hydrogen-enriched ion exchange material with the liquid resource under conditions suitable to absorb lithium to generate a lithium-enriched ion exchange material; (d) optionally, washing the lithium-enriched ion exchange material with water to generate a lithium-enriched ion exchange material substantially free of liquid resource; and (e) repeating the cycle to produce a lithium-enriched solution from the liquid resource.
[0270] In some embodiments, the process of extracting lithium occurs by contacting solutions described above with an ion exchange material occurs within one or more of the devices for lithium extraction disclosed herein.
[0271] In one aspect described herein, is a process for lithium extraction from a liquid resource comprising treating ion exchange material alternately with acid, brine, and optionally other solutions, in a configuration where the ion exchange material moves in the net opposite direction to the acid, brine, and optionally other solutions, thereby producing a lithium-enriched solution from the liquid resource. In one aspect described herein, is a process for lithium extraction from a liquid resource comprising treating ion exchange material alternately with acid, the liquid resource, and optionally other solutions, in a configuration where the ion exchange materialWSGR Docket No. 50741-727.601moves in the net opposite direction to the acid, liquid resource, and optionally other solutions, thereby producing a lithium-enriched solution from the liquid resource. In one aspect described herein, is a process for lithium extraction from a liquid resource comprising treating ion exchange material alternately with acid, brine, and optionally other solutions, in a configuration where the ion exchange material moves in the net opposite direction to the acid, brine, and optionally other solutions, thereby producing a lithium-enriched solution from the brine. In one embodiment, the process comprises: (a) treating the ion exchange material with acid under conditions suitable to absorb hydrogen to generate hydrogen-enriched material and release lithium to generate a lithium-enriched solution; (b) optionally, washing the hydrogen-enriched material with water to generate hydrogen-enriched material substantially free of residual acid; (c) treating the hydrogen-enriched material with the liquid resource under conditions suitable to absorb lithium to generate lithium-enriched material; (d) optionally, washing the lithium-enriched material with water to generate lithium-enriched beads substantially free of liquid resource; and (e) repeating the cycle to produce a lithium-enriched solution from the liquid resource.
[0272] In one embodiment, the ion exchange material comprises ion exchange particles that reversibly exchange lithium and hydrogen and a structural matrix material, and having a pore network. In one embodiment, the liquid resource comprises a natural brine, a dissolve salt flat, a concentrated brine, a processed brine, a filtered brine, a liquid from an ion exchange process, a liquid from a solvent extraction process, a synthetic brine, leachate from ores, leachate from minerals, leachate from clays leachate from recycled products, leachate from recycled materials, or combinations thereof.
[0273] In some embodiments herein, is a process for lithium extraction from a liquid resource comprising treating an ion exchange material alternately with acid, brine, and optionally other solutions, in a configuration where the material move in the net opposite direction to the acid, brine, and optionally other solutions, thereby producing a lithium-enriched solution from the liquid resource, wherein the process comprises: a) treating the an ion exchange material with acid under conditions suitable to absorb hydrogen to generate hydrogen-enriched material and release lithium to generate a lithium-enriched solution; b) optionally, washing the hydrogen-enriched material with water to generate hydrogen-enriched beads substantially free of residual acid; c) treating the hydrogen-enriched beads with the liquid resource under conditions suitable to absorb lithium to generate lithium-enriched beads; d) optionally, washing the lithium-enriched beads with water to generate lithium-enriched beads substantially free of liquidWSGR Docket No. 50741-727.601resource; and e) repeating the cycle to produce a lithium-enriched solution from the liquid resource.
[0274] In one aspect described herein, is a process for lithium extraction from a liquid resource comprising treating ion exchange particles alternately with the liquid resource, washing fluid, and acid, in a system for the extraction of lithium ions from a liquid resource, comprising: a) an ion exchange material; b) a ion exchange vessel; and c) a pH modulating setup for increasing the pH of the liquid resource in the system.
[0275] In one aspect described herein, is a process for lithium extraction from a liquid resource comprising treating ion exchange particles alternately with the liquid resource, a washing fluid, and an acid solution, with a system for the extraction of lithium ions from a liquid resource, comprising a stirred rank reactor, an ion exchange material, a pH modulating setup for increasing the pH of the liquid resource in the ion exchange vessel, and a compartment for containing the ion exchange material in the ion exchange vessel while allowing for removal of liquid resource, washing fluid, and acid solutions from the ion exchange vessel.Process of modulating pH for the extraction of lithium
[0276] An aspect of the disclosure herein is a process for the extraction of lithium ions from a liquid resource, comprising: a) contacting an ion exchange material with the liquid resource; and b) increasing the pH of the liquid resource before contact with the ion exchange material, during contact with the ion exchange material, after contact with the ion exchange material and combinations thereof.
[0277] In some embodiment, the process of contacting a liquid resource with an ion exchange material occurs within one or more of the devices for lithium extraction disclosed herein. In some embodiments, several such devices are connected, and the liquid resource undergoes a treatment to increase its pH when flowing from one such vessel to the next.
[0278] Another aspect described herein is a process for the extraction of lithium ions from a liquid resource, comprising: a) contacting an ion exchange material with the liquid resource; and b) increasing the pH of the liquid resource before contact with the ion exchange material, during contact with the ion exchange material, after contact with the ion exchange material, or combinations thereof. In some embodiments of the process, increasing the pH of the liquid resource is before contacting the ion exchange material with the liquid resource. In some embodiments of the process, increasing the pH of the liquid resource is during contacting the ion exchange material with the liquid resource. In some embodiments of the process, increasing the pH of the liquid resource is after contacting the ion exchange material with the liquid resource.WSGR Docket No. 50741-727.601In some embodiments of the process, increasing the pH of the liquid resource is before and during contacting the ion exchange material with the liquid resource. In some embodiments of the process, increasing the pH of the liquid resource is before and after contacting the ion exchange material with the liquid resource. In some embodiments of the process, increasing the pH of the liquid resource is during and after contacting the ion exchange material with the liquid resource. In some embodiments of the process, increasing the pH of the liquid resource is before, during, and after contacting the ion exchange material with the liquid resource.
[0279] An aspect of the disclosure herein is a process, wherein the ion exchange material is loaded into a column. In an embodiment, the process further comprises: a) loading a liquid resource into one or more liquid resource tanks; b) connecting the column to the one or more liquid resource tanks; and c) passing the liquid resource from the one or more liquid resource tanks through the column, wherein the passing of the liquid resource occurs at least once. In an embodiment, the process further comprises increasing the pH of the liquid resource in one or more pH increasing tanks. In an embodiment, the process further comprises settling precipitates in one or more settling tanks. In an embodiment, the process further comprises storing the liquid resource in one or more storing tanks prior to or after circulating the liquid resource through the column.
[0280] An aspect of the disclosure herein is a process, wherein the process further comprises: a) loading the liquid resource into one or more liquid resource tanks; b) connecting the column to the one or more liquid resource tanks; c) passing the liquid resource from the one or more liquid resource tanks through the column, wherein the passing of the liquid resource occurs at least once; d) increasing the pH of the liquid resulting from c. in one or more pH increasing tanks; e) settling precipitates of the liquid resulting from d. in one or more settling tanks; and f) storing the liquid resulting from e. in one or more storing tanks.
[0281] An aspect of the disclosure herein is a process, wherein the ion exchange material is loaded in a plurality of columns. In an embodiment, a plurality of tanks is connected to the plurality of columns, wherein each of the plurality of tanks is immediately connected to one of the plurality of columns. In an embodiment, two or more of the plurality of columns forms at least one circuit. In an embodiment, at least one circuit is selected from a liquid resource circuit, a water washing circuit and an acid solution circuit. In an embodiment, the pH of the liquid resource is increased in the plurality of tanks connected to the plurality of columns in the liquid resource circuit. In an embodiment, the liquid resource circuit includes a plurality of columns connected to a plurality of tanks, wherein each of the plurality of tanks is immediately connected to one of the plurality of columns.WSGR Docket No. 50741-727.601
[0282] An aspect of the disclosure herein is a process, wherein the process further comprises: a) passing the liquid resource through a plurality of columns in the liquid resource circuit; b) passing an acid solution through a plurality of columns in the acid solution circuit one or more times; and c) passing water through a plurality of columns in the water washing circuit. In an embodiment, the process further comprises interchanging a plurality of columns between the liquid resource circuit, the water washing circuit and the acid solution circuit, such that: a) at least one of the plurality of columns in the liquid resource circuit becomes at least one of the plurality of columns in the water washing circuit and / or at least one of the plurality of columns in the acid solution circuit; b) at least one of the plurality of columns in the water washing circuit becomes at least one of the plurality of columns in the acid solution circuit and / or at least one of the plurality of columns in the liquid resource circuit; and / or c) at least one of the plurality of columns in the acid solution circuit becomes at least one of the plurality of columns in the liquid resource circuit and / or at least one of the plurality of columns in the water washing circuit.
[0283] An aspect of the disclosure herein is a process, wherein the ion exchange material is loaded into one or more compartments in a tank. In an embodiment, the process further comprises moving the liquid resource through the one or more compartments in the tank. In an embodiment, the tank comprises injection ports. In an embodiment, the process further comprises using the injection ports to increase the pH of the liquid resource before contact with the ion exchange material, during contact with the ion exchange material, after contact with the ion exchange material and combinations thereof.
[0284] In some embodiments, the process further comprises using the injection ports to increase the pH of the liquid resource before contact with the ion exchange material, during contact with the ion exchange material, after contact with the ion exchange material, or combinations thereof.
[0285] An aspect of the disclosure herein is a process, wherein the column further comprises a plurality of injection ports. In an embodiment, the process further comprises using the plurality of injection ports to increase the pH of the liquid resource before contact with the ion exchange material, during contact with the ion exchange material, after contact with the ion exchange material and combinations thereof.
[0286] In some embodiments, the process further comprises using the plurality of injection ports to increase the pH of the liquid resource before contact with the ion exchange material, during contact with the ion exchange material, after contact with the ion exchange material, or combinations thereof.WSGR Docket No. 50741-727.601
[0287] In an embodiment, the ion exchange material comprises a plurality of ion exchange particles. In an embodiment, the plurality of ion exchange particles in the ion exchange material is selected from uncoated ion exchange particles, coated ion exchange particles and combinations thereof. In an embodiment, the ion exchange material is an ion exchange material. In an embodiment, the ion exchange material comprises a network of pores that allows liquids to move quickly from the surface of the ion exchange material to the plurality of ion exchange particles. In an embodiment, the ion exchange material is in the form of an ion exchange material.
[0288] In an embodiment, the ion exchange material extracts lithium ions from a liquid resource. During the extraction of lithium ions from a liquid resource by the ion exchange material, the pH of the liquid resource optionally decreases. Increasing the pH of the liquid resource in the system maintains the pH in a range that is suitable for lithium ion uptake by the ion exchange material. In an embodiment, increasing the pH comprises measuring the pH of the system and adjusting the pH of the system to an ideal pH range for lithium extraction. In an embodiment, for ion exchange material to absorb lithium from brine, an ideal pH range for the brine is optionally 6 to 9, a preferred pH range is optionally 4 to 9, and an acceptable pH range is optionally 2 to 9. In an embodiment, increasing the pH comprises measuring the pH of the system and wherein the pH of the system is less than 6, less than 4, or less than 2, the pH of the system is adjusted to a pH of 2 to 9, a pH of 4 to 9, or a pH of 6 to 9.The liquid resource
[0289] In some embodiments, the liquid resource is selected from the following list: a natural brine, a dissolved salt flat, a geothermal brine, seawater, concentrated seawater, desalination effluent, a concentrated brine, a processed brine, liquid from an ion exchange process, liquid from a solvent extraction process, a synthetic brine, leachate from ores, leachate from minerals, leachate from clays, leachate from sediments, leachate from recycled products, leachate from recycled materials, or combinations thereof. In some embodiments, a liquid resource is selected from the following list: a natural brine, a dissolved salt flat, a concentrated brine, a processed brine, a synthetic brine, a geothermal brine, liquid from an ion exchange process, liquid from a solvent extraction process, leachate from minerals, leachate from clays, leachate from recycled products, leachate from recycled materials, or combinations thereof. In some embodiments, the liquid resource is optionally pre-treated prior to entering the ion exchange reactor to remove suspended solids, hydrocarbons, organic molecules, iron, certain metals, or other chemical or ionic species. In some embodiments, the liquid resource is optionally fed into the ion exchangeWSGR Docket No. 50741-727.601reactor without any pre-treatment following from its source. In some embodiments, the liquid resource is injected into a reservoir, salt lake, salt flat, basin, or other geologic deposit after lithium has been removed from the liquid resource. In some embodiments, other species are recovered from the liquid resource before or after lithium recovery. In some embodiments, the pH of the liquid resource is adjusted before, during, or after lithium recovery.
[0290] In one embodiment, the liquid resource is a natural brine, a dissolved salt flat, seawater, concentrated seawater, a geothermal brine, a desalination effluent, a concentrated brine, a processed brine, an oilfield brine, a liquid from an ion exchange process, a liquid from a solvent extraction process, a synthetic brine, a leachate from an ore or combination of ores, a leachate from a mineral or combination of minerals, a leachate from a clay or combination of clays, a leachate from recycled products, a leachate from recycled materials, or combinations thereof.
[0291] In one embodiment, the brine is at a temperature of -20 to 20 C, 20 to 50 C, 50 to 100 C, 100 to 200 C, or 200 to 400 C. In one embodiment, the brine is heated or cooled to precipitate or dissolve species in the brine, or to facilitate removal of metals from the brine.
[0292] In one embodiment, the brine contains lithium at a concentration of less than 1 mg / L, 1 to 50 mg / L, 50 to 200 mg / L, 200 to 500 mg / L, 500 to 2,000 mg / L, 2,000 to 5,000 mg / L, 5,000 to 10,000 mg / L, 10,000 to 20,000 mg / L, 20,000 to 80,000 mg / L, or greater than 80,000 mg / L.
[0293] In one embodiment, the brine contains magnesium at a concentration of 0.01 to 0.1 mg / L, 0.1 to 1 mg / L, 1 to 10 mg / L, 10 to 100 mg / L, 100 to 1,000 mg / L, 1,000 to 10,000 mg / L, 10,000 to 50,000 mg / L, 50,000 to 100,000 mg / L, 100,000 to 150,000 mg / L, or greater than 150,000 mg / L. In one embodiment, the brine contains calcium at a concentration of 0.01 to 0.1 mg / L, 0.1 to 1 mg / L, 1 to 10 mg / L, 10 to 100 mg / L, 100 to 1,000 mg / L, 1,000 to 10,000 mg / L, 10,000 to 50,000 mg / L, 50,000 to 100,000 mg / L, 100,000 to 150,000 mg / L, or greater than 150,000 mg / L. In one embodiment, the brine contains strontium at a concentration of 0.01 to 0.1 mg / L, 0.1 to 1 mg / L, 1 to 10 mg / L, 10 to 100 mg / L, 100 to 1,000 mg / L, 1,000 to 10,000 mg / L, 10,000 to 50,000 mg / L, 50,000 to 100,000 mg / L, 100,000 to 150,000 mg / L, or greater than 150,000 mg / L. In one embodiment, the brine contains barium at a concentration of 0.01 to 0.1 mg / L, 0.1 to 1 mg / L, 1 to 10 mg / L, 10 to 100 mg / L, 100 to 1,000 mg / L, 1,000 to 10,000 mg / L, 10,000 to 50,000 mg / L, 50,000 to 100,000 mg / L, 100,000 to 150,000 mg / L, or greater than 150,000 mg / L.
[0294] In one embodiment, the brine contains multivalent cations at a concentration of 0.01 to 0.1 mg / L, 0.1 to 1 mg / L, 1 to 10 mg / L, 10 to 100 mg / L, 100 to 1,000 mg / L, 1,000 to 10,000 mg / L, 10,000 to 50,000 mg / L, 50,000 to 100,000 mg / L, 100,000 to 150,000 mg / L, or greater than 150,000 mg / L. In one embodiment, the brine contains multivalent ions at a concentration ofWSGR Docket No. 50741-727.6010.01 to 0.1 mg / L, 0.1 to 1 mg / L, 1 to 10 mg / L, 10 to 100 mg / L, 100 to 1,000 mg / L, 1,000 to 10,000 mg / L, 10,000 to 50,000 mg / L, 50,000 to 100,000 mg / L, 100,000 to 150,000 mg / L, or greater than 150,000 mg / L. In one embodiment, the brine contains non-lithium impurities at a concentration of 0.01 to 0.1 mg / L, 0.1 to 1 mg / L, 1 to 10 mg / L, 10 to 100 mg / L, 100 to 1,000 mg / L, 1,000 to 10,000 mg / L, 10,000 to 50,000 mg / L, 50,000 to 100,000 mg / L, 100,000 to 150,000 mg / L, or greater than 150,000 mg / L. In one embodiment, the brine contains transition metals at a concentration of 0.01 to 0.1 mg / L, 0.1 to 1 mg / L, 1 to 10 mg / L, 10 to 100 mg / L, 100 to 1,000 mg / L, 1,000 to 10,000 mg / L, 10,000 to 50,000 mg / L, 50,000 to 100,000 mg / L, 100,000 to 150,000 mg / L, or greater than 150,000 mg / L. In one embodiment, the brine contains iron at a concentration of 0.01 to 0.1 mg / L, 0.1 to 1 mg / L, 1 to 10 mg / L, 10 to 100 mg / L, 100 to 1,000 mg / L, 1,000 to 10,000 mg / L, 10,000 to 50,000 mg / L, 50,000 to 100,000 mg / L, 100,000 to 150,000 mg / L, or greater than 150,000 mg / L. In one embodiment, the brine contains manganese at a concentration of 0.01 to 0.1 mg / L, 0.1 to 1 mg / L, 1 to 10 mg / L, 10 to 100 mg / L, 100 to 1,000 mg / L, 1,000 to 10,000 mg / L, 10,000 to 50,000 mg / L, 50,000 to 100,000 mg / L, 100,000 to 150,000 mg / L, or greater than 150,000 mg / L.
[0295] In one embodiment, the brine is treated to produce a feed brine which has certain metals removed. In one embodiment, the feed brine contains iron at a concentration of less than 0.01, 0.01 to 0.1 mg / L, mg / L, 0.1 to 1.0 mg / L, 1.0 to 10 mg / L, 10 to 100 mg / L, or 100 to 1,000 mg / L. In one embodiment, the feed brine contains manganese at a concentration of less than 0.01, 0.01 to 0.1 mg / L, mg / L, 0.1 to 1.0 mg / L, 1.0 to 10 mg / L, 10 to 100 mg / L, or 100 to 1,000 mg / L. In one embodiment, the feed brine contains lead at a concentration of less than 0.01, 0.01 to 0.1 mg / L, mg / L, 0.1 to 1.0 mg / L, 1.0 to 10 mg / L, 10 to 100 mg / L, or 100 to 1,000 mg / L. In one embodiment, the feed brine contains zinc at a concentration of less than 0.01, 0.01 to 0.1 mg / L, mg / L, 0.1 to 1.0 mg / L, 1.0 to 10 mg / L, 10 to 100 mg / L, or 100 to 1,000 mg / L. In one embodiment, the feed brine contains lithium at a concentration of 1 to 50 mg / L, 50 to 200 mg / L, 200 to 500 mg / L, 500 to 2,000 mg / L, or greater than 2,000 mg / L.
[0296] In one embodiment, the feed brine is processed to recover metals such as lithium and yield a spent brine or raffinate. In one embodiment, the raffinate contains residual quantities of the recovered metals at a concentration of less than 0.01, 0.01 to 0.1 mg / L, mg / L, 0.1 to 1.0 mg / L, 1.0 to 10 mg / L, 10 to 100 mg / L, 100 to 1,000 mg / L, or 1,000 to 10,000 mg / L.
[0297] In one embodiment, the pH of the brine is corrected to less than 0, 0 to 1, 1 to 2, 2 to 4, 4 to 6, 6 to 8, 4 to 8, 8 to 9, 9 to 10, 9 to 11, or 10 to 12. In one embodiment, the pH of the brine is corrected to 2 to 4, 4 to 6, 6 to 8, 4 to 8, 8 to 9, 9 to 10, 9 to 11, or 10 to 12. In one embodiment, the pH of the brine is corrected to precipitate or dissolve metals.WSGR Docket No. 50741-727.601
[0298] In one embodiment, metals are precipitated from the brine to form precipitates. In one embodiment, precipitates include transition metal hydroxides, oxy -hydroxides, sulfide, flocculants, aggregate, agglomerates, or combinations thereof. In one embodiment, the precipitates include Li, Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti,, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Mn, Tc, Fe, Fe, Ru, Os, Co, Rh, Ir, Ni, Pd Pt, Cu, Ag, Au, Zn, Cd, Hg, B, Al, Ga, In, Si, Ge, Sn, Pb, As, Sb, Bi, Se, Te, Po, Br, I, At, other metals, or a combination thereof. In one embodiment, the precipitates are concentrated into a slurry, a filter cake, a wet filter cake, a dry filter cake, a dense slurry, or a dilute slurry.
[0299] In one embodiment, the precipitates contain iron at a concentration of less than 0.01 mg / kg, 0.01 to 1 mg / kg, 1 to 100 mg / kg, 100 to 10,000 mg / kg, or 10,000 to 800,000 mg / kg. In one embodiment, the precipitates contain manganese at a concentration of less than 0.01 mg / kg, 0.01 to 1 mg / kg, 1 to 100 mg / kg, 100 to 10,000 mg / kg, or 10,000 to 800,000 mg / kg. In one embodiment, the precipitates contain lead at a concentration of less than 0.01 mg / kg, 0.01 to 1 mg / kg, 1 to 100 mg / kg, 100 to 10,000 mg / kg, or 10,000 to 800,000 mg / kg. In one embodiment, the precipitates contain arsenic at a concentration of less than 0.01 mg / kg, 0.01 to 1 mg / kg, 1 to 100 mg / kg, 100 to 10,000 mg / kg, or 10,000 to 800,000 mg / kg. In one embodiment, the precipitates contain magnesium at a concentration of less than 0.01 mg / kg, 0.01 to 1 mg / kg, 1 to 100 mg / kg, 100 to 10,000 mg / kg, or 10,000 to 800,000 mg / kg. In one embodiment, the precipitates contain Li, Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti,, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Mn, Tc, Fe, Fe, Ru, Os, Co, Rh, Ir, Ni, Pd Pt, Cu, Ag, Au, Zn, Cd, Hg, B, Al, Ga, In, Si, Ge, Sn, Pb, As, Sb, Bi, Se, Te, Po, Br, I, At, or other metals at a concentration of less than 0.01 mg / kg, 0.01 to 1 mg / kg, 1 to 100 mg / kg, 100 to 10,000 mg / kg, or 10,000 to 800,000 mg / kg. In one embodiment, the precipitates are toxic and / or radioactive.
[0300] In one embodiment, precipitates are redissolved by combining the precipitates with acid. In one embodiment, precipitates are redissolved by combining the precipitates with acid in a mixing apparatus. In one embodiment, precipitates are redissolved by combining the precipitates with acid using a high-shear mixer.
[0301] Lithium is an essential element for batteries and other technologies. Lithium is found in a variety of liquid resources, including natural and synthetic brines and leachate solutions from minerals, clays, and recycled products. Lithium is optionally extracted from such liquid resources using an ion exchange process based on inorganic ion exchange materials. These inorganic ion exchange materials absorb lithium from a liquid resource while releasing hydrogen, and then elute lithium into an acidic solution while absorbing hydrogen. This ion exchange process is optionally repeated to extract lithium from a liquid resource and yield aWSGR Docket No. 50741-727.601concentrated lithium solution. The concentrated lithium solution is optionally further processed into chemicals for the battery industry or other industries.
[0302] Ion exchange materials are optionally formed into beads and the beads are optionally loaded into ion exchange columns, stirred tank reactors, other reactors, or other systems for lithium extraction. Alternating flows or aliquots of brine, acidic solution, and optionally other solutions are flowed through or flowed into an ion exchange column, reactors, or reactor system to extract lithium from the brine and produce a lithium concentrate, which is eluted from the column using the acidic solution. As brine flows through the ion exchange column, reactors, or reactor system, the ion exchange material absorbs lithium while releasing hydrogen, where both the lithium and hydrogen are cations. The release of hydrogen during lithium uptake will acidify the brine and limit lithium uptake unless the pH of the brine is optionally maintained in a suitable range to facilitate thermodynamically favorable lithium uptake and concomitant hydrogen release. In one embodiment, pH of the liquid resource is maintained near a set-point through addition of base to neutralized protons released from the ion exchange material into the liquid resource.Treatment of the liquid resource
[0303] In some embodiments, the pH of the liquid resource is adjusted before, during and / or after contact with the lithium-selective ion exchange material to maintain the pH in range that is suitable for lithium uptake.
[0304] To control the pH of the brine and maintain the pH in a range that is suitable for lithium uptake in an ion exchange column, bases such as NaOH, Ca(OH)2, CaO, KOH, or NH3are optionally added to the brine as solids, aqueous solutions, or in other forms. For brines that contain divalent ions such as Mg, Ca, Sr, or Ba, addition of base to the brine can cause precipitation of solids, such as Mg(OH)2or Ca(OH)2, which can cause problems for the ion exchange reaction. These precipitates cause problems in at least three ways. First, precipitation can remove base from solution, leaving less base available in solution to neutralize protons and maintain pH in a suitable range for lithium uptake in the ion exchange column. Second, precipitates that form due to base addition can clog the ion exchange column, including clogging the surfaces and pores of an ion exchange material and the voids between an ion exchange material. This clogging can prevent lithium from entering the beads and being absorbed by the ion exchange material. The clogging can also cause large pressure heads in the column. Third, precipitates in the column dissolve during acid elution and thereby contaminate the lithium concentrate produced by the ion exchange system. For an ion exchange material to absorbWSGR Docket No. 50741-727.601lithium from brine, an ideal pH range for the brine is optionally 5 to 7, a preferred pH range is optionally 4 to 8, and an acceptable pH range is optionally 1 to 9. In one embodiment, an pH range for the brine is optionally about 1 to about 14, about 2 to about 13, about 3 to about 12, about 4 to about 12, about 4.5 to about 11, about 5 to about 10, about 5 to about 9, about 2 to about 5, about 2 to about 4, about 2 to about 3, about 3 to about 8, about 3 to about 7, about 3 to about 6, about 3 to about 5, about 3 to about 4, about 4 to about 10, about 4 to about 9, about 4 to about 8, about 4 to about 7, about 4 to about 6, about 4 to about 5, about 5 to about 6, about 5 to about 7, about 5 to about 8, about 6 to about 7, about 6 to about 8, or about 7 to about 8.
[0305] In one embodiment, the liquid resource is subjected to treatment prior to ion exchange. In some embodiments, said treatment comprises filtration, gravity sedimentation, centrifugal sedimentation, magnetic fields, other methods of solid-liquid separation, or combinations thereof. In some embodiments, precipitated metals are removed from the brine using a filter. In some embodiments, the filter is a belt filter, plate-and-frame filter press, pressure vessel containing filter elements, rotary drum filter, rotary disc filter, cartridge filter, a centrifugal filter with a fixed or moving bed, a metal screen, a perforated basket centrifuge, a three-point centrifuge, a peeler type centrifuge, or a pusher centrifuge. In some embodiments, the filter may use a scroll or a vibrating device. In some embodiments, the filter is horizontal, vertical, or may use a siphon.
[0306] In some embodiments, a filter cake is prevented, limited, or removed by using gravity, centrifugal force, an electric field, vibration, brushes, liquid jets, scrapers, intermittent reverse flow, vibration, crow-flow filtration, or pumping suspensions across the surface of the filter. In some embodiments, the precipitated metals and a liquid is moved tangentially to the filter to limit cake growth. In some embodiments, gravitational, magnetic, centrifugal sedimentation, or other means of solid-liquid separation are used before, during, or after filtering to prevent cake formation.
[0307] In some embodiments, a filter comprises a screen, a metal screen, a sieve, a sieve bend, a bent sieve, a high frequency electromagnetic screen, a resonance screen, or combinations thereof. In some embodiments, one or more particle traps are a solid-liquid separation apparatus.
[0308] In some embodiments, one or more solid-liquid separation apparatuses are used in series or parallel. In some embodiments, a dilute slurry is removed from the tank, transferred to an external solid-liquid separation apparatus, and separated into a concentrated slurry and a solution with low or no suspended solids. In some embodiments, the concentrated slurry is returned to the tank or transferred to a different tank. In some embodiments, precipitate metals are transferred from a brine tank to another brine tank, from an acid tank to another acid tank, fromWSGR Docket No. 50741-727.601a washing tank to another washing tank, from a brine tank to a washing tank, from a washing tank to an acid tank, from an acid tank to a washing tank, or from an acid tank to a brine tank.
[0309] In some embodiments, solid-liquid separation apparatuses may use gravitational sedimentation. In some embodiments, solid-liquid separation apparatuses may include a settling tank, a thickener, a clarifier, a gravity thickener. In some embodiments, solid-liquid separation apparatuses are operated in batch mode, semi -batch mode, semi-continuous mode, or continuous mode. In some embodiments, solid-liquid separation apparatuses include a circular basin thickener with slurry entering through a central inlet such that the slurry is dispersed into the thickener with one or more raking components that rotate and concentrate the ion exchange particles into a zone where the particles can leave through the bottom of the thickener.
[0310] In some embodiments, solid-liquid separation apparatuses include a deep cone, a deep cone tank, a deep cone compression tank, or a tank wherein the slurry is compacted by weight. In some embodiments, solid-liquid separation apparatuses include a tray thickener with a series of thickeners oriented vertically with a center axle and raking components. In some embodiments, solid-liquid separation apparatuses include a lamella type thickener with inclined plates or tubes that are smooth, flat, rough, or corrugated. In some embodiments, solid-liquid separation apparatuses include a gravity clarifier that is a rectangular basin with feed at one end and overflow at the opposite end optionally with paddles and / or a chain mechanism to move particles. In some embodiments, the solid-liquid separation apparatuses are a particle trap.
[0311] In some embodiments, the solid-liquid separation apparatuses use centrifugal sedimentation. In some embodiments, solid-liquid separation apparatuses may include a tubular centrifuge, a multi-chamber centrifuge, a conical basket centrifuge, a scroll-type centrifuge, a sedimenting centrifuge, or a disc centrifuge. In some embodiments, precipitated metals are discharged continuously or intermittently from the centrifuge. In some embodiments, the solidliquid separation apparatus is a hydrocyclone. In some embodiments, solid-liquid separation apparatus is an array of hydrocyclones or centrifuges in series and / or in parallel. In some embodiments, sumps are used to reslurry the precipitated metals. In some embodiments, the hydrocyclones have multiple feed points. In some embodiments, a hydrocyclone is used upside down. In some embodiments, liquid is injected near the apex of the cone of a hydrocyclone to improve sharpness of cut. In some embodiments, a weir rotates in the center of the particle trap with a feed of slurried precipitated metals entering near the middle of the apparatus, and precipitated metals get trapped at the bottom and center of the apparatus due to a “teacup effect”.WSGR Docket No. 50741-727.601Vessels for beds of an ion exchange material
[0312] For commercial production of lithium using ion exchange, it is desirable to construct large-scale ion exchange modules containing large quantities of an ion exchange material.However, most large vessels capable of holding about one tonne or more of an ion exchange material have large fluid flow distances of about one meter or more. These fluid flow distances cause large pressure drops. To reduce the pressure drop across the ion exchange bed, the ion exchange material are loaded into vessels facilitating flow across the ion exchange material with a shorter fluid flow distance. These vessels are designed to evenly distribute flow of the liquid resource and other fluids through the ion exchange material. In some embodiments, these vessels minimize the distance that the fluid flows as it contacts the ion exchange material.
[0313] In some embodiments, the vessel is oriented vertically, horizontally, or at any angle relative to the horizontal axis. In some embodiments, the vessel is cylindrical, rectangular, spherical, another shape, or a combinations thereof. In some embodiments, the vessel can have a constant cross-sectional area or a varying cross-sectional area.
[0314] In some embodiments, the vessel has a height to diameter ratio of less than about 0.1, 0.5, less than about 1, less than about 2, less than about 5, less than about 10, more than about 0.1, more than about 0.5, more than about 1, more than about 2, more than about 5, more than about 10. In one embodiment, the vessel internal is coated with a polymeric or rubber material. In one embodiment the vessel is equipped with an outlet collector tray. In one embodiment the vessel has multiple injection ports for the inlet or outlet flow. In one embodiment the flow is introduced from the bottom, top, middle of the vessel, or a combination of thereof. In one embodiment the vessel is outfitted with baffles or plates to break fluid jets.An ion exchange material contained within vessels with minimal flow distance
[0315] In some embodiments, vessels containing the ion exchange material are designed to minimize the distance that the fluid flows as it contacts the ion exchange material. In some embodiments, said design minimizes the energy required to contact a fluid with the ion exchange material. In some embodiments, said fluid is a liquid resource, a washing solution, a solution containing a chemical additive, or an acidic eluent solution.
[0316] In some embodiments, the ion exchange material contained within such a vessel have an average particle diameter less than about 10 pm, less than about 20 pm, less than about 30 pm, less than about 40 pm, less than about 50 pm, less than about 60 pm, less than about 70 pm, less than about 80 pm, less than about 90 pm, less than about 100 pm, less than about 200 pm, less than about 300 pm, less than about 400 pm, less than about 500 pm, less than about 600 pm,WSGR Docket No. 50741-727.601less than about 700 µm, less than about 800 µm, less than about 900 µm, less than about 1000 µm, less than about 2000 µm. In some embodiments, the ion exchange material have an average particle diameter more than about 10 µm, more than about 20 µm, more than about 30 µm, more than about 40 µm, more than about 50 µm, more than about 60 µm, more than about 70 µm, more than about 80 µm, more than about 90 µm, more than about 100 µm, more than about 200 µm, more than about 300 µm, more than about 400 µm, more than about 500 µm, more than about 600 µm, more than about 700 µm, more than about 800 µm, more than about 900 µm, more than about 1000 µm, more than about 2000 µm. In some embodiments, the ion exchange material have a typical particle size from about 10 µm to about 20 µm, from about 20 µm to about 40 µm, from about 40 µm to about 80 µm, from about 80 µm to about 200 µm, from about 100 µm to about 400 µm, from about 200 µm to about 800 µm, from about 400 µm to about 1000 µm, from about 600 µm to about 2000 µm, from about 1000 µm to about 2000 µm.Methods of modulating pH for the extraction of lithium
[0317] An aspect of the disclosure provided herein is a method of extracting lithium ions from a liquid resource, comprising: flowing the liquid resource through the column of the system described above to produce a lithiated ion exchange material; and treating the resulting lithiated ion exchange material with an acid solution to produce a salt solution comprising lithium ions.
[0318] An aspect of the disclosure provided herein is a method of extracting lithium ions from a liquid resource, comprising: flowing the liquid resource through the plurality of columns of the system described above to produce a lithiated ion exchange material; and treating the resulting lithiated ion exchange material with an acid solution to produce a salt solution comprising lithium ions.
[0319] An aspect of the disclosure provided herein is a method of extracting lithium ions from a liquid resource, comprising: flowing the liquid resource through the tank of the system described above to produce a lithiated ion exchange material; and treating the resulting lithiated ion exchange material with an acid solution to produce a salt solution comprising lithium ions.
[0320] An aspect of the disclosure provided herein is a method of extracting lithium ions from a liquid resource, comprising: flowing the liquid resource through the column of the system described above to produce a lithiated ion exchange material; and treating the resulting lithiated ion exchange material with an acid solution to produce a salt solution comprising lithium ions.
[0321] In some embodiments, the liquid resource is selected from the following list: a natural brine, a dissolved salt flat, a geothermal brine, seawater, concentrated seawater, desalination effluent, a concentrated brine, a processed brine, liquid from an ion exchange process, liquidWSGR Docket No. 50741-727.601from a solvent extraction process, a synthetic brine, leachate from ores, leachate from minerals, leachate from clays, leachate from recycled products, leachate from recycled materials, or combinations thereof. In some embodiments, a liquid resource is selected from the following list: a natural brine, a dissolved salt flat, a concentrated brine, a processed brine, a synthetic brine, a geothermal brine, liquid from an ion exchange process, liquid from a solvent extraction process, leachate from minerals, leachate from clays, leachate from recycled products, leachate from recycled materials, or combinations thereof. In some embodiments, the liquid resource is optionally pre-treated prior to entering the ion exchange reactor to remove suspended solids, hydrocarbons, or organic molecules. In some embodiments, the liquid resource is optionally entered the ion exchange reactor without any pre-treatment following from its source.
[0322] In an embodiment, the liquid resource is a natural brine, a dissolved salt flat, seawater, concentrated seawater, a desalination effluent, a concentrated brine, a processed brine, an oilfield brine, a liquid from an ion exchange process, a liquid from a solvent extraction process, a synthetic brine, a leachate from an ore or combination of ores, a leachate from a mineral or combination of minerals, a leachate from a clay or combination of clays, a leachate from recycled products, a leachate from recycled materials, or combinations thereof.
[0323] In some embodiments, the liquid resource is selected with a lithium concentration selected from the following list: less than 100,000 ppm, less than 10,000 ppm, less than 1,000 ppm, less than 100 ppm, less than 10 ppm, or combinations thereof. In some embodiments, a liquid resource is selected with a lithium concentration selected from the following list: less than 5,000 ppm, less than 500 ppm, less than 50 ppm, or combinations thereof.
[0324] In some embodiments, the acid used for recovering lithium from the ion exchange reactor is selected from the following list: hydrochloric acid, sulfuric acid, phosphoric acid, hydrobromic acid, chloric acid, perchloric acid, nitric acid, formic acid, carbonic acid, acetic acid, or combinations thereof. In some embodiments, the acid used for recovering lithium from the porous an ion exchange material is selected from the following list: hydrochloric acid, sulfuric acid, nitric acid, carbonic acid, acetic acid, or combinations thereof.
[0325] In an embodiment, the acid solution comprises hydrochloric acid, sulfuric acid, phosphoric acid, hydrobromic acid, chloric acid, perchloric acid, nitric acid, formic acid, carbonic acid, acetic acid, or combinations thereof.
[0326] In some embodiments, the acid used for recovering lithium from the ion exchange system has a concentration selected from the following list: less than 0.1 M, less than 1.0 M, less than 5 M, less than 10 M, or combinations thereof. In some embodiments, the acid used forWSGR Docket No. 50741-727.601recovering lithium from the porous an ion exchange material has a concentration greater than 10 M.
[0327] In an embodiment, acids with distinct concentrations are used during the elution process. In an embodiment, acid with a lower concentration is first added to elute lithium from the ion exchange material and then additional acid of a greater concentration is added to elute more lithium into the solution and increase the concentration of lithium in the eluate.
[0328] In some embodiments, the ion exchange material perform the ion exchange reaction repeatedly while maintaining adequate lithium uptake capacity over a number of cycles selected from the following list: greater than 10 cycles, greater than 30 cycles, greater than 100 cycles, greater than 300 cycles, or greater than 1,000 cycles. In some embodiments, the porous an ion exchange material perform the ion exchange reaction repeatedly over a number of cycles selected from the following list: greater than 50 cycles, greater than 100 cycles, or greater than 200 cycles. In some embodiments, adequate lithium uptake capacity is optionally defined as a percentage of initial uptake capacity selected from the following list: greater than 95%, greater than 90%, greater than 80%, greater than 60%, or greater than 20%. In some embodiments, adequate lithium uptake capacity is optionally defined as a percentage of initial uptake capacity such as less than 20%.
[0329] In some embodiments, the concentrated lithium solution that is yielded from the ion exchange reactor is further processed into lithium raw materials using methods selected from the following list: solvent extraction, ion exchange, chemical precipitation, electrodialysis, electrowinning, electrolysis, evaporation with direct solar energy, evaporation with concentrated solar energy, evaporation with a heat transfer medium heated by concentrated solar energy, evaporation with heat from a geothermal brine, evaporation with heat from combustion, pH neutralization, or combinations thereof. In some embodiments, the concentrated lithium solution that is yielded from the ion exchange reactor is concentrated using reverse osmosis or membrane technologies.
[0330] In some embodiments, the concentrated lithium solution that is yielded from the ion exchange reactor is further processed into lithium chemicals selected from the following list: lithium chloride, lithium carbonate, lithium hydroxide, lithium metal, lithium metal oxide, lithium metal phosphate, lithium sulfide, or combinations thereof. In some embodiments, the concentrated lithium solution that is yielded from the porous an ion exchange material is further processed into lithium chemicals that are solid, liquid, hydrated, or anhydrous.
[0331] In some embodiments, the lithium chemicals produced using the ion exchange reactor are used in an industrial application selected from the following list: lithium batteries, metalWSGR Docket No. 50741-727.601alloys, glass, grease, or combinations thereof. In some embodiments, the lithium chemicals produced using the coated ion exchange particles are used in an application selected from the following list: lithium batteries, lithium-ion batteries, lithium sulfur batteries, lithium solid-state batteries, and combinations thereof.
[0332] In some embodiments, the ion exchange materials are synthesized in a lithiated state with a sublattice fully or partly occupied by lithium. In some embodiments, the ion exchange materials are synthesized in a hydrated state with a sublattice fully or partly occupied by hydrogen.
[0333] In some embodiments, the ion exchange material extracts lithium ions from a liquid resource. During the extraction of lithium ions from a liquid resource by the ion exchange material, the pH of the liquid resource optionally decreases. Increasing the pH of the liquid resource in the system by using a pH modulating setup maintains the pH in a range that is suitable for lithium ion uptake by the ion exchange material. In an embodiment, the pH modulating setup comprises measuring the pH of the system and adjusting the pH of the system to an ideal pH range for lithium extraction. In an embodiment, for ion exchange material to absorb lithium from brine, an ideal pH range for the brine is optionally 6 to 9, a preferred pH range is optionally 4 to 9, and an acceptable pH range is optionally 2 to 9. In an embodiment, the pH modulating setup comprises measuring the pH of the system and wherein the pH of the system is less than 6, less than 4, or less than 2, the pH of the system is adjusted to a pH of 2 to 9, a pH of 4 to 9, or a pH of 6 to 9.
[0334] Another aspect described herein is a method of extracting lithium ions from a liquid resource, comprising: a) flowing the liquid resource into a system comprising a tank to produce a lithiated ion exchange mateiral, wherein the tank further comprises (i) one or more compartments, (ii) an ion exchange material, (iii) a mixing device, and (iv) a pH modulating setup for changing the pH of the liquid resource in the system; and b) treating the lithiated ion exchange material from a) with an acid solution to produce a hydrogen-rich ion exchange material and a salt solution comprising lithium ions.
[0335] In some embodiments, the method further comprises, prior to b), washing the lithiated ion exchange material with an aqueous solution. In some embodiments, the method further comprises, subsequent to b), washing the hydrogen-rich ion exchange material with an aqueous solution. In some embodiments, the aqueous solution is water.
[0336] In some embodiments, the method further comprises, prior to b), flowing the lithiated ion exchange material into a washing system. In some embodiments, the method further comprises, prior to b), transferring a suspension comprising the lithiated ion exchange material. In someWSGR Docket No. 50741-727.601embodiments, the method further comprises, prior to b), flowing the lithiated ion exchange material into a washing system and washing the lithiated ion exchange material with a solution. In some embodiments, the method further comprises, prior to b), flowing the lithiated ion exchange material into a washing system and washing the lithiated ion exchange material with a solution comprising water. In some embodiments, the method further comprises, prior to b), flowing the lithiated ion exchange material into a washing system and washing the lithiated ion exchange material with an aqueous solution. In some embodiments, the lithiated ion exchange material is washed with an aqueous solution.
[0337] In some embodiments, the method further comprises, prior to b), flowing the lithiated ion exchange material into a stripping system. In some embodiments, the method further comprises, prior to b), flowing the lithiated ion exchange material into a stripping system and stripping the lithiated ion exchange material. In some embodiments, the method further comprises, prior to b), flowing the lithiated ion exchange material into a stripping system and stripping volatile components from the lithiated ion exchange material. In some embodiments, the method further comprises, prior to b), flowing the lithiated ion exchange material into a stripping system and stripping volatile components comprising water from the lithiated ion exchange material.
[0338] In some embodiments, the pH modulating setup comprises a pH measuring device and an inlet for adding base to the tank. In some embodiments, the pH measuring device is a pH probe. In some embodiments, the inlet is a pipe. In some embodiments, the inlet is an injection port.
[0339] In some embodiments, the method further comprises, during a), measuring a change in pH of the liquid resource using the pH modulating setup. In some embodiments, the measured change in pH triggers adding a base to maintain lithium uptake. In some embodiments, a change in pH to below a pH value of about 2 to about 9 triggers the addition of a base to maintain lithium uptake. In some embodiments, a change in pH to below a pH value of about 2, of about 3, of about 4, of about 5, of about 6, of about 7, of about 8, or of about 9 triggers the addition of a base to maintain lithium uptake. In some embodiments, a change in pH to below a pH of about 2 to about 4, of about 3 to about 5, of about 4 to about 6, of about 5 to about 7, of about 6 to about 8, or of about 7 to about 9 triggers the addition of a base to maintain lithium uptake. In some embodiments, base is added to the liquid resource to maintain the pH of the liquid resource in a range of about 2-3, 3-4, 4-5, 5-6, 6-7, 7-8, or 8-9. In some embodiments, base is added to the liquid resource to maintain the pH of the liquid resource in a range of about 4-5, 5-6, 6-7, or 7-8. In some embodiments, base is added to the liquid resource to maintain the pH of the liquid resource in a range of about 4.0-4.5, 4.5-5.0, 5.0-5.5, 5.5-6.0, 6.0-6.5, 6.5-7.0, 7.0-7.5, or 7.5-WSGR Docket No. 50741-727.6018.0. In some embodiments, the pH of a liquid resource is maintained in a target range that is high enough to facilitate lithium uptake and low enough to avoid precipitation of metal salts from the liquid resource. In some embodiments, the pH of a liquid resource is maintained below a pH of about 8 to avoid precipitation of Mg salts. In some embodiments, the pH of a liquid resource is maintained below a pH of about 2, below a pH of about 3, below a pH of about 4, below a pH of about 5, below a pH of about 6, below a pH of about 7, below a pH of about 8, or below a pH of about 9 to avoid precipitation of metal salts. In some embodiments, the pH of the liquid resource may drop out of a target pH range due to release of protons from an ion exchange material and a pH modulating setup may adjust the pH of the liquid resource back to within a target pH range. In some embodiments, the pH of the liquid resource is adjusted above a target pH range prior to the liquid resource entering the system and then protons released from the ion exchange material may decrease the pH of the system into the target range. In some embodiments, the pH of the liquid resource is controlled in a certain range and the range is changed over time. In some embodiments, the pH of the liquid resource is controlled in a certain range and then the pH of the liquid resource is allowed to drop. In some embodiments, the pH of the liquid resource is controlled in a certain range and then the pH of the liquid resource is allowed to drop to solubilize colloids or solids. In some embodiments, base is added to a liquid resource to neutralize protons without measuring pH. In some embodiments, base is added to a liquid resource to neutralize protons with monitoring of volumes or quantities of the base. In some embodiments, the pH of the liquid resource is measured to monitor lithium uptake by an ion exchange material. In some embodiments, the pH of the liquid resource is monitored to determine when to separate a liquid resource from an ion exchange material. In some embodiments, the rate of change of the pH of the liquid resource is measured to monitor the rate of lithium uptake. In some embodiments, the rate of change of the pH of the liquid resource is measured to determine when to separate a liquid resource from an ion exchange material.
[0340] In some embodiments, the tank further comprises a porous partition. In some embodiments, the method further comprises, after a), draining the liquid resource through the porous partition after the production of the lithiated ion exchange material (e.g., the lithium-rich ion exchange material). In some embodiments, the method further comprises, after b), draining the salt solution comprising lithium ions through the porous partition after the production of the hydrogen-rich ion exchange material (e.g., the ion exchange material).
[0341] In some embodiments, the method further comprises, subsequent to a), flowing the lithiated ion exchange material into another system comprising a tank to produce the hydrogen-WSGR Docket No. 50741-727.601rich ion exchange material and the salt solution comprising lithium ions, wherein the tank of the other system further comprises (i) one or more compartments, and (ii) a mixing device.
[0342] In some embodiments, the system comprises a plurality of tanks and each of the plurality of tanks further comprises (i) one or more compartments, (ii) an ion exchange material, (iii) a mixing device, and (iv) a pH modulating setup for changing the pH of the system.
[0343] An aspect described herein is a method of extracting lithium ions from a liquid resource, comprising: a) flowing the liquid resource into a first system comprising a tank, wherein the tank of the first system further comprises (i) one or more compartments, (ii) an ion exchange material, (iii) a mixing device, and (iv) a pH modulating setup for changing the pH of the liquid resource in the first system, to produce a lithiated ion exchange material; b) flowing the lithiated ion exchange material of a) into a second system comprising a tank, wherein the tank of the second system further comprises (i) one or more compartments, and (ii) a mixing device; and c) treating the lithiated ion exchange from b) with an acid solution to produce a hydrogen-rich ion exchange material and a salt solution comprising lithium ions.
[0344] In some embodiments, the method further comprises, subsequent to a), washing the lithiated ion exchange material with an aqueous solution.
[0345] In some embodiments, the method further comprises, prior to b), adding an aqueous solution to the lithiated ion exchange material to form a fluidized lithiated ion exchange material.
[0346] In some embodiments, the method further comprises, subsequent to c), washing the hydrogen-rich ion exchange material with an aqueous solution. In some embodiments, the aqueous solution is water.
[0347] In some embodiments, the pH modulating setup comprises a pH measuring device and an inlet for adding base. In some embodiments, the pH measuring device is a pH probe. In some embodiments, the inlet is a pipe. In some embodiments, the inlet is an injection port.
[0348] In some embodiments, the method further comprises, during a), measuring a change in pH of the liquid resource using the pH modulating setup. In some embodiments, the change in pH triggers adding a base to maintain lithium uptake.
[0349] An aspect described herein is a method of extracting lithium ions from a liquid resource, comprising: a) flowing the liquid resource into a first system comprising a plurality of tanks to produce a lithiated ion exchange material, wherein each of the plurality of tanks in the first system is in fluid communication with every other one of the plurality of tanks in the first system and, each of the plurality of tanks in the first system further comprises (i) one or more compartments, (ii) an ion exchange material, (iii) a mixing device, and (iv) a pH modulatingWSGR Docket No. 50741-727.601setup for changing the pH of each of the plurality of tanks in the first system; b) flowing the lithiated ion exchange material into a second system comprising a plurality of tanks, wherein each of the plurality of tanks in the second system is in fluid communication with every other one of the plurality of tanks in the second system and, each of the plurality of tanks in the second system further comprises (i) one or more compartments, and (ii) a mixing device; and c) treating the lithiated ion exchange material from b) with an acid solution in at least one of the plurality of tanks in the second system to produce a hydrogen-rich ion exchange material and a salt solution comprising lithium ions.
[0350] In some embodiments, the method further comprises, subsequent to c), washing the hydrogen-rich ion exchange material with an aqueous solution in at least one of the plurality of tanks in the second system.
[0351] In some embodiments, the method is operated in a batch mode. In some embodiments, the method is operated in a continuous mode. In some embodiments, the method is operated in continuous and batch mode. In some embodiments, the method is operated in continuous mode, a batch mode, a semi-continuous mode, or combinations thereof.
[0352] In some embodiments, the pH modulating setup comprises a pH measuring device and an inlet for adding base. In some embodiments, the pH measuring device is a pH probe. In some embodiments, the inlet is a pipe. In some embodiments, the inlet is an injection port.
[0353] In some embodiments, the method further comprises, during a), measuring a change in pH of the liquid resource using the pH modulating setup. In some embodiments, the change in pH triggers adding a base to maintain lithium uptake.
[0354] An aspect described herein is a method of extracting lithium ions from a liquid resource, comprising: a) flowing the liquid resource into a first system comprising a tank to produce a lithiated ion exchange material, wherein the tank further comprises (i) one or more compartments, (ii) ion exchange material, and (iii) a mixing device; b) flowing the lithiated ion exchange material from a) into a second system comprising a tank, wherein the tank further comprises (i) one or more compartments, (ii) an acid solution, and (iii) a mixing device; and c) stripping the lithiated ion exchange material to produce hydrogen-rich ion exchange material and a salt solution comprising lithium ions.
[0355] In some embodiments, prior to b), the lithiated ion exchange material is washed. In some embodiments, the lithiated ion exchange material is washed with an aqueous solution.
[0356] An aspect described herein is a method of extracting lithium ions from a liquid resource, comprising: a) providing a system comprising an ion exchange material, a tank comprising one or more compartments; and a mixing device, wherein (i) the ion exchange material is oxide-WSGR Docket No. 50741-727.601based and exchanges hydrogen ions with lithium ions, and (ii) the mixing device is capable of moving the liquid resource around the tank comprising one or more compartments; b) flowing the liquid resource into the system of a), thereby contacting the liquid resource with the ion exchange material, wherein the ion exchange material exchanges hydrogen ions with lithium ions in the liquid resource to produce lithiated ion exchange material; c) removing the liquid resource from the system of b); d) flowing an acid solution into the system of c) thereby contacting the acid solution with the lithiated ion exchange material, wherein the lithiated ion exchange material exchanges lithium ions with the hydrogen ions in the acid solution to produce the ion exchange material and a salt solution comprising lithium ions from the lithiated ion exchange material; and e) collecting the salt solution comprising the lithium ions for further processing.
[0357] In some embodiments, the salt solution comprising lithium ions undergoes crystallization.
[0358] A method of extracting lithium ions from a liquid resource, comprising: a) flowing the liquid resource through a system comprising an ion exchange material and a plurality of columns, wherein the plurality of columns is configured to transport the ion exchange material along the length of the column, to produce a lithiated ion exchange material; and b) treating the lithiated ion exchange material from a) with an acid solution to produce a salt solution comprising lithium ions.
[0359] An aspect described herein is a method of extracting lithium ions from a liquid resource, comprising: a) providing a system comprising an ion exchange material and a plurality of columns, wherein each of the plurality of columns is configured to transport the ion exchange material along the length of the column; b) flowing the liquid resource through a first one of the plurality of columns to produce a lithiated ion exchange material; c) flowing the lithiated ion exchange material from b) into a second one of the plurality of columns; and d) treating the lithiated ion exchange material from c) with an acid solution to produce a hydrogen-rich ion exchange material and a salt solution comprising lithium ions.
[0360] In some embodiments, the method further comprises, subsequent to b), flowing the lithiated ion exchange material into another one of the plurality of columns and washing the lithiated ion exchange material with an aqueous solution. In some embodiments, the method further comprises, subsequent to d), flowing the hydrogen-rich ion exchange material into another one of the plurality of columns and washing the hydrogen-rich ion exchange material with an aqueous solution.WSGR Docket No. 50741-727.601
[0361] An aspect described herein is a method of extracting lithium ion from a liquid resource, comprising: a) providing a system comprising an ion exchange material and a plurality of columns, wherein each of the plurality of columns is configured to transport the ion exchange material along the length of the column; b) flowing the liquid resource through a first one of the plurality of columns to produce a lithiated ion exchange material; c) flowing the lithiated ion exchange material from b) into a second one of the plurality of columns; d) washing the lithiated ion exchange material from c) with an aqueous solution; e) flowing the lithiated ion exchange material from d) into a third one of the plurality of columns; and f) treating the lithiated ion exchange material from e) with an acid solution to produce a hydrogen-rich ion exchange material and a salt solution comprising lithium ions.
[0362] In some embodiments, the method further comprises: g) flowing the hydrogen-rich ion exchange material into a fourth one of the plurality of columns; and h) washing the hydrogenrich ion exchange material with an aqueous solution. In some embodiments, each of the plurality of columns is configured to transport the ion exchange material by a pipe system or an internal conveyer system. In some embodiments, each of the plurality of columns is configured to transport the ion exchange material by a pipe system. In some embodiments, each of the plurality of columns is configured to transport the ion exchange material by an internal conveyer system.
[0363] In some embodiments of the methods described herein, the liquid resource is a natural brine, a dissolved salt flat, seawater, concentrated seawater, a desalination effluent, a concentrated brine, a processed brine, waste brine from a bromine-extraction process, an oilfield brine, a liquid from an ion exchange process, a liquid from a solvent extraction process, a synthetic brine, a leachate from an ore or combination of ores, a leachate from a mineral or combination of minerals, a leachate from a clay or combination of clays, a leachate from recycled products, a leachate from recycled materials, or combinations thereof. In some embodiments of the methods described herein, the liquid resource is a brine. In some embodiments of the methods described herein, the liquid resource comprises a natural brine, a synthetic brine, or a mixture of a natural and a synthetic brine. In some embodiments of the methods described herein, the liquid resource is a natural brine, a dissolved salt flat, seawater, concentrated seawater, a desalination effluent, a concentrated brine, a processed brine, waste brine from a bromine-extraction process, an oilfield brine, a liquid from an ion exchange process, or combinations thereof.
[0364] In some embodiments of the methods and systems provided herein, the eluent or eluent solution is an acid solution (e.g., an acidic solution). In some embodiments of the methodsWSGR Docket No. 50741-727.601described herein, the acid solution comprises hydrochloric acid, sulfuric acid, phosphoric acid, hydrobromic acid, chloric acid, perchloric acid, nitric acid, formic acid, carbonic acid, acetic acid, or combinations thereof. In some embodiments of the methods described herein, the acid solution comprises hydrochloric acid, sulfuric acid, phosphoric acid, nitric acid, or combinations thereof. In some embodiments of the methods described herein, the acid solution comprises hydrochloric acid, sulfuric acid, phosphoric acid, or combinations thereof. In some embodiments of the methods described herein the acid solution comprises hydrochloric acid. In some embodiments of the methods described herein the acid solution comprises sulfuric acid. In some embodiments of the methods described herein the acid solution comprises phosphoric acid. In some embodiments of the methods described herein the acid solution comprises carbonic acid.Numbered Embodiments of the Disclosure
[0365] Below are provided some non-limiting embodiments of the present disclosure:Embodiment 1. A method for preparing a mixed metal compound and reducing gas emissions, the method comprising:(a) contacting a metal salt precursor with a metal precursor to generate a mixture; (b) heating said mixture to form the mixed metal compound, wherein said heating generates a by-product gas from decomposition of the metal salt precursor, the metal precursor, or any combination thereof;(c) absorbing said by-product gas into an absorber solution to generate an absorbed gas solution; and(d) processing said absorbed gas solution to produce a metal salt precursor, a metal precursor, or any combination thereof.Embodiment 2. The method of Embodiment 1, wherein the metal salt precursor produced by the method of (d) comprises the same metal salt precursor used to generate the mixture of (a).Embodiment 3. The method of Embodiment 1 or 2, wherein the metal precursor produced by the method of (d) comprises the same the metal precursor used to generate the mixture of (a).Embodiment 4. The method of Embodiment 1, wherein the metal salt precursor comprises lithium sulfate, lithium carbonate, lithium hydroxide, lithium phosphate, lithium nitrate, sodium nitrate, sodium sulfate, sodium carbonate, sodium hydroxide, sodium phosphate, modifications thereof, solid solutions thereof, or combinations thereof.WSGR Docket No. 50741-727.601Embodiment 5. The method of Embodiment 1, wherein the metal salt precursor comprises lithium nitrate, lithium sulfate, lithium phosphate, sodium nitrate, sodium sulfate, sodium phosphate, modifications thereof, solid solutions thereof, or combinations thereof.Embodiment 6. The method of Embodiment 1, wherein the metal salt precursor comprises lithium nitrate, lithium sulfate, modifications thereof, solid solutions thereof, or combinations thereof.Embodiment 7. The method of Embodiment 1, wherein the metal salt precursor comprises lithium nitrate.Embodiment 8. The method of Embodiment 1, wherein the metal salt precursor comprises lithium sulfate.Embodiment 9. The method of any one of Embodiments 1 to 8, wherein the metal precursor comprises titanium dioxide, titanium alkoxides, manganese dioxide, manganese oxide, manganese carbonate, manganese acetate, manganese hydroxide, tin oxide, tin acetate, tin sulfate, copper oxide, aluminum oxide, vanadium oxide, manganese nitrate, manganese sulfate, manganese phosphate, iron phosphate, ferric nitrate, ferric sulfate, ferrous nitrate, ferrous sulfate, iron oxide, cobalt oxide, NixMnyCo1-x-y(OH)2, NixMnyAl1-x-y(OH)2, solid solutions thereof, or combinations thereof.Embodiment 10. The method of any one of Embodiments 1 to 9, wherein the mixed metal compound comprises LiFePO4, LiMnPO4U, Li2TiO3, Li2MnO3, Li2SnO3, Li4Ti5O12, Li4Mn5O12, LiMn2O4, Li1.6Mn1.6O4, LiAlO2, LiCuO2, LiTiO2, Li4TiO4, Li7Ti11O24, Li3VO4, Li2CuP2O7, LiNixMnyCoi-x-yO2, LiNixMnyAli-x-y02, modifications thereof, solid solutions thereof, or a combination thereof.Embodiment 11. The method of any one of Embodiments 1 to 10, wherein the mixed metal compound is an ion exchange material, which reversibly exchanges lithium and hydrogen ions.Embodiment 12. The method of any one of Embodiments 1 to 11, wherein the cationic molar ratio of metal salt precursor to the metal precursor in the mixture of step (a) is from about 0.5:1 to 0.8:1.Embodiment 13. The method of any one of Embodiments 1 to 11, wherein the cationic molar ratio of metal salt precursor to the metal precursor in the mixture of step (a) is from about 0.8:1 to 1:1.Embodiment 14. The method of any one of Embodiments 1 to 11, wherein the cationic molar ratio of metal salt precursor to the metal precursor in the mixture of step (a) is from about 1:1 to 1.2:1.WSGR Docket No. 50741-727.601Embodiment 15. The method of any one of Embodiments 1 to 11, wherein the cationic molar ratio of metal salt precursor to the metal precursor in the mixture of step (a) is from about 1.2:1 to 2:1.Embodiment 16. The method of any one of Embodiments 1 to 11, wherein the cationic molar ratio of metal salt precursor to the metal precursor in the mixture of step (a) is from about 2: 1 to 4: 1.Embodiment 17. The method of any one of Embodiments 1 to 16, wherein step (b) occurs in a pusher kiln, a roller hearth kiln, a rotary kiln, a rotary furnace, a muffle furnace, a batch furnace, or a continuous furnace.Embodiment 18. The method of any one of Embodiments 1 to 17, wherein step (b) occurs at a temperature between about 250 and 2250 °C.Embodiment 19. The method of any one of Embodiments 1 to 17, wherein step (b) occurs at a temperature between about ...
Claims
WSGR Docket No. 50741-727.601CLAIMS WHAT IS CLAIMED IS:
1. A method for preparing a mixed metal compound and reducing gas emissions, the method comprising:(a) contacting a metal salt precursor with a metal precursor to generate a mixture; (b) heating said mixture to form the mixed metal compound, wherein said heating generates a by-product gas from decomposition of the metal salt precursor, the metal precursor, or any combination thereof;(c) absorbing said by-product gas into an absorber solution to generate an absorbed gas solution; and(d) processing said absorbed gas solution to produce the metal salt precursor, the metal precursor, or any combination thereof.
2. The method of claim 1, wherein the metal salt precursor produced by the method of (d) comprises the same metal salt precursor used to generate the mixture of (a).
3. The method of claim 1 or 2, wherein the metal precursor produced by the method of (d) comprises the same the metal precursor used to generate the mixture of (a).
4. The method of any one of claims 1 to 3, wherein the metal salt precursor comprises lithium sulfate, lithium carbonate, lithium hydroxide, lithium phosphate, lithium nitrate, sodium nitrate, sodium sulfate, sodium carbonate, sodium hydroxide, sodium phosphate, modifications thereof, solid solutions thereof, or combinations thereof.
5. The method of any one of claims 1 to 3, wherein the metal salt precursor comprises lithium nitrate, lithium sulfate, lithium phosphate, sodium nitrate, sodium sulfate, sodium phosphate, modifications thereof, solid solutions thereof, or combinations thereof.
6. The method of any one of claims 1 to 3, wherein the metal salt precursor comprises lithium nitrate, lithium sulfate, modifications thereof, solid solutions thereof, or combinations thereof.
7. The method of any one of claims 1 to 3, wherein the metal salt precursor comprises lithium nitrate.
8. The method of any one of claims 1 to 3, wherein the metal salt precursor comprises lithium sulfate.
9. The method of any one of claims 1 to 8, wherein the metal precursor comprises titanium dioxide, titanium alkoxides, manganese dioxide, manganese oxide, manganese carbonate, manganese acetate, manganese hydroxide, tin oxide, tin acetate, tin sulfate, copper oxide, aluminum oxide, vanadium oxide, manganese nitrate, manganese sulfate, manganeseWSGR Docket No. 50741-727.601phosphate, iron phosphate, ferric nitrate, ferric sulfate, ferrous nitrate, ferrous sulfate, iron oxide, cobalt oxide, NixMnyCo1-x-y(OH)2, NixMnyAl1-x-y(OH)2, solid solutions thereof, or combinations thereof.
10. The method of any one of claims 1 to 8, wherein the metal precursor comprises TiO2, MnO2, MnCO3, or combinations thereof.
11. The method of any one of claims 1 to 8, wherein the metal precursor comprises MnO2or MnCO3.
12. The method of any one of claims 1 to 11, wherein the mixed metal compound is an ion exchange material, which reversibly exchanges lithium and hydrogen ions.
13. The method of any one of claims 1 to 12, wherein the mixed metal compound comprises LiFePO4, LiMnPO4U, Li2TiO3, Li2MnO3, Li2SnO3, Li4Ti5O12, Li4Mn5O12, LiMn2O4, Li1.6Mn1.6O4, LiAlCL, LiCuCL, LiTiO2, Li4TiO4, Li? TinO24, Li3VO4, Li2CuP2O7, LiNixMnyCoi-x-yO2, LiNixMnyAli-x-y02, modifications thereof, solid solutions thereof, or a combination thereof.
14. The method of any one of claims 1 to 12, wherein the mixed metal compound comprises Li2TiO3, Li2MnO3, Li4Ti5O12, Li4Mn30i2, i n2O4, Li1.6 n1.eO4, LiTiO2, Li4TiO4, Li7Ti11O24, modifications thereof, solid solutions thereof, or a combination thereof.
15. The method of any one of claims 1 to 12, wherein the mixed metal compound comprises Li4Ti5O12or Li4Mn5O12.
16. The method of any one of claims 1 to 15, further comprising applying a coating to the mixed metal compound to form a coated mixed metal compound.
17. The method of claim 16, wherein the coating is an oxide material, a polymer material, or a combination thereof.
18. The method of claim 16 or 17, wherein the polymer material comprises polyvinylidene difluoride, polyvinyl chloride, a fluoro-polymer, a chloro-polymer, a fluoro-chloro-polymer, or combinations thereof.
19. The method of claim 16 or 17, wherein the oxide material comprises TiO2, ZrO2, SiO2, Al2O3, solid solutions thereof, or combinations thereof.
20. The method of any one of claims 1 to 19, wherein the cationic molar ratio of metal salt precursor to the metal precursor in the mixture of step (a) is from about 0.5:1 to 0.8:1.
21. The method of any one of claims 1 to 19, wherein the cationic molar ratio of metal salt precursor to the metal precursor in the mixture of step (a) is from about 0.8: 1 to 1: 1.
22. The method of any one of claims 1 to 19, wherein the cationic molar ratio of metal salt precursor to the metal precursor in the mixture of step (a) is from about 1:1 to 1.2:1.WSGR Docket No. 50741-727.60123. The method of any one of claims 1 to 19, wherein the cationic molar ratio of metal salt precursor to the metal precursor in the mixture of step (a) is from about 1.2: 1 to 2: 1.
24. The method of any one of claims 1 to 19, wherein the cationic molar ratio of metal salt precursor to the metal precursor in the mixture of step (a) is from about 2:1 to 4: 1.
25. The method of any one of claims 1 to 24, wherein step (b) occurs in a pusher kiln, a roller hearth kiln, a rotary kiln, a rotary furnace, a muffle furnace, a batch furnace, or a continuous furnace.
26. The method of any one of claims 1 to 25, wherein step (b) occurs at a temperature between about 250 and 2250 °C.
27. The method of any one of claims 1 to 25, wherein step (b) occurs at a temperature between about 250 and 1000 °C.
28. The method of any one of claims 1 to 25, wherein step (b) occurs at a temperature between about 250 and 500 °C.
29. The method of any one of claims 1 to 25, wherein step (b) occurs at a temperature between about 500 and 1000°C.
30. The method of any one of claims 1 to 25, wherein step (b) occurs at a temperature between about 400 and 950°C.
31. The method of any one of claims 1 to 30, wherein step (b) occurs with two stages at different temperatures.
32. The method of claim 31, wherein the first stage of the heating occurs at a temperature between about 200 and 300 °C and the second stage of heating occurs at a temperature between about 400 and 500 °C.
33. The method of claim 31, wherein the first stage of the heating occurs at a temperature between about 250 and 500 °C and the second stage of the heating occurs at a temperature between about 600 and 800 °C.
34. The method of claim 31, wherein the first stage of the heating occurs at a temperature between about 250 and 500 °C and the second stage of the heating occurs at a temperature between about 800 and 1000 °C.
35. The method of any one of claims 1 to 34, wherein the heating occurs within a controlled gas atmosphere supplied by fresh gas comprising air, oxygen, nitrogen, or combinations thereof.
36. The method of claim 35, wherein the controlled gas atmosphere has a fresh gas exchange rate between about 5 and 150 vessel volumes per hour.
37. The method of any one of claims 1 to 36, wherein the by-product gas comprises NOX, SOX, or combinations thereof.WSGR Docket No. 50741-727.60138. The method of claim 37, wherein the by-product gas comprises NOX.
39. The method of claim 37, wherein the by-product gas comprises SOX.
40. The method of any one of claims 1 to 39, wherein step (c) occurs in a wet absorber system.
41. The method of claim 40, wherein said wet absorber system comprises a packed tower absorber, a spray tower absorber, a venturi absorber, a tray-type absorber, or combinations thereof.
42. The method of any one of claims 1 to 41, wherein the by-product gas is oxidized prior to absorption by passing the by-product gas over a catalyst bed in the presence oxygen gas.
43. The method of any one of claims 1 to 42, wherein the by-product gas is oxidized prior to absorption by mixing the by-product gas with an oxidizing gas, wherein the oxidizing gas comprises chlorine, ozone, oxygen, or combinations thereof.
44. The method of any one of claims 1 to 43, wherein the by-product gas is oxidized during the absorption process with the inclusion of an oxidizer in the absorber solution.
45. The method of claim 44, wherein the oxidizer comprises H2O2.
46. The method of any one of claims 1 to 45, wherein the absorbed gas solution of step (c) comprises an aqueous solution of sulfuric acid, nitric acid, hydrogen peroxide, or combinations thereof.
47. The method of claim 45 or 46, wherein the hydrogen peroxide concentration is maintained during absorption at a level of at least about 1 wt%.
48. The method of claim 45 or 46, wherein the hydrogen peroxide concentration is maintained during absorption at a level of at least about 2 wt%.
49. The method of claim 45 or 46, wherein the hydrogen peroxide concentration is maintained during absorption at a level of at least about 3 wt%.
50. The method of any one of claims 45 to 49, wherein the hydrogen peroxide concentration is no more than about 35 wt%.
51. The method of any of the claims 45 to 50, wherein the hydrogen peroxide concentration is no more than about 25 wt%.
52. The method of any one of claims 46 to 51, wherein the nitric acid concentration is at least about 1 wt%.
53. The method of any one of claims 46 to 51, wherein the nitric acid concentration is at least about 2 wt%.
54. The method of any one of claims 46 to 51, wherein the nitric acid concentration is at least about 3 wt%.WSGR Docket No. 50741-727.60155. The method of any one of claims 46 to 51, wherein the nitric acid concentration is no more than about 10 wt%.
56. The method of any of the claims 46 to 51, wherein the nitric acid concentration is no more than about 25 wt%.
57. The method of any of the claims 46 to 51, wherein the nitric acid concentration is no more than about 35 wt%.
58. The method of any of the claims 46 to 51, wherein the nitric acid concentration is no more than about 45 wt%.
59. The method of any one of claims 46 to 58, wherein the sulfuric acid concentration is at least about 1 wt%.
60. The method of any one of claims 46 to 58, wherein the sulfuric acid concentration is at least about 2 wt%.
61. The method of any one of claims 46 to 58, wherein the sulfuric acid concentration is at least about 3 wt%.
62. The method of any one of claims 46 to 58, wherein the sulfuric acid concentration is no more than about 10 wt%.
63. The method of any of the claims 46 to 58, wherein the sulfuric acid concentration is from about 99 to 100 wt%.
64. The method of any of the claims 46 to 58, wherein the sulfuric acid concentration is at least about 97 wt%.
65. The method of any one of claims 1 to 64 wherein the absorber solution in step (c) comprises an aqueous lithium hydroxide solution.
66. The method of any one of claims 1 to 65, wherein the absorbed gas solution from step (c) comprises lithium nitrite and is mixed with hydrogen peroxide to oxidize the nitrite anions to nitrate.
67. The method of any one of claims 1 to 66, wherein the absorbed gas solution from step (c) comprises lithium sulfite and is mixed with a hydrogen peroxide to oxidize the sulfite anions to sulfate.
68. The method of any one of claims 1 to 67, wherein the by-product gas recovery rate in step (c) is at least about 95%.
69. The method of any one of claims 1 to 67, wherein the by-product gas recovery rate in step (c) is at least about 97%.
70. The method of any one of claims 1 to 67, wherein the by-product gas recovery rate in step (c) is at least about 99%.WSGR Docket No. 50741-727.60171. The method of any one of claims 1 to 70, wherein the absorbed gas solution from step (c) is transferred to a conversion process wherein lithium carbonate and lithium hydroxide are added to the absorber solution comprising nitric acid to produce a lithium nitrate.
72. The method of any one of claims 1 to 71, wherein the absorbed gas solution from step (c) is transferred to a conversion process wherein lithium hydroxide is added to the absorber solution comprising sulfuric acid to produce a lithium sulfate.
73. The method of claim 71 or 72, wherein the molar ratio (atomic Li basis) of lithium carbonate to lithium hydroxide added ranges from about 90: 10 to 97:3.
74. The method of claim 71 or 72, wherein the molar ratio (atomic Li basis) of lithium carbonate to lithium hydroxide added ranges from about 10:90 to 90:10.
75. The method of claim 71 or 72, wherein the molar ratio (atomic Li basis) of lithium carbonate to lithium hydroxide added ranges from about 0:100 to 10:90.
76. The method of any one of claims 1 to 75, wherein the pH of the absorbed gas solution from step (c) is raised to at least about 9 to induce precipitation of impurities as metal hydroxides.
77. The method of any one of claims 1 to 75, wherein the pH of the absorbed gas solution from step (c) is raised to at least about 10 to induce precipitation of impurities as metal hydroxides.
78. The method of any one of claims 1 to 75, wherein the pH of the absorbed gas solution from step (c) is raised to at least about 11 to induce precipitation of impurities as metal hydroxides.
79. The method of any one of claims 1 to 78, wherein the absorbed gas solution from step (c) is filtered after addition of lithium salts using equipment comprising filter presses, cartridge filters, bag filters, candle filters, membrane filters, or combinations thereof, to produce a filtered absorbed gas solution.
80. The method of claim 79, wherein the pH of the filtered absorbed gas solution is lowered to pH 7 after filtration.
81. The method of claim 79, wherein the pH of the filtered absorbed gas solution is lowered to pH 5 after filtration.
82. The method of claim 79, wherein the pH of the filtered absorbed gas solution is lowered to pH 3.5 after filtration.
83. The method of any one of claims 79 to 82, wherein the filtered absorbed gas solution is passed through a divalent ion-exchange process to remove divalent cations comprising calcium, magnesium, strontium, barium, or combinations thereof.WSGR Docket No. 50741-727.60184. The method of any one of claims 79 to 83, wherein the filtered absorbed gas solution is concentrated with process equipment comprising reverse osmosis membrane systems, nanofiltration membrane systems, mechanical vapor recompression evaporators, singleeffect evaporators, multiple effect evaporators, falling film evaporators, forced circulation evaporators, modifications thereof, or combinations thereof.
85. The method of any one of claims 79 to 84, wherein the filtered absorbed gas solution is crystallized to produce a slurry using equipment comprising a cooling crystallizer, an agitated tank crystallizer, a forced circulation crystallizer, a draft tube crystallizer, modifications thereof, or combinations thereof, wherein the slurry comprises a solid crystal salt and a mother liquor.
86. The method of claim 85, wherein the solid crystal salt from the slurry is separated from the mother liquor using equipment comprising a centrifuge, a pusher centrifuge, a peeler centrifuge, a basket centrifuge, a filter press, a continuous centrifuge, a batch centrifuge, or combinations thereof.
87. The method of claim 86, wherein the mother liquor is recycled back to the crystallization process.
88. The method of claim 86, wherein the mother liquor is recycled back to the concentration process.
89. The method of claim 86, wherein the solid crystal salt is dried in equipment comprising a fluid bed dryer, a vacuum tray dryer, a forced circulation tray dryer, a vacuum belt dryer, a vacuum rotary dryer, a hollow flight screw conveyor dryer, or combinations thereof.
90. A method of forming a porous bead, the method comprising:(a) forming a mixed metal compound or a coated mixed metal compound according to the method of any one of claims 1 to 89, and(b) combining the mixed metal compound or the coated mixed metal compound with a matrix material,wherein said mixed metal compound or said coated mixed metal compound is embedded in, adhered to, or otherwise supported by the matrix material to form the porous bead.
91. The method of claim 90, wherein the matrix material comprises a polymer, an oxide, a phosphate, or combinations thereof.
92. The method of claim 90 or 91, wherein the porous bead comprises pores with diameters ranging from more than 1 μm to less than 100 μm.WSGR Docket No. 50741-727.60193. The method of any one of claims 90 to 92, wherein the matrix material comprises polyvinylidene fluoride, polyvinyl fluoride, polyvinyl chloride, polyvinylidene chloride, a chloro-polymer, a fluoro-polymer, a fluoro-chloro-polymer, polyethylene, polypropylene, polyphenylene sulfide, polytetrafluoroethylene, sulfonated polytetrafluoroethylene, polystyrene, polydivinylbenzene, polybutadiene, a sulfonated polymer, a carboxylated polymer, polyacrylonitrile, perfluoro-3,6-dioxa-4-methyl-7-octene-sulfonic acid (Nafion®), copolymers thereof, or combinations thereof.
94. The method of any one of claims 90 to 93, wherein the matrix material comprises one or more oxides.
95. The method of claim 94, wherein said one or more oxides comprise silica, alumina, zirconia, titania, natural clay (e.g. Bentonite), or any combination thereof.
96. The method of any of the claims 1 to 95, wherein the mixed metal compound, the coated mixed metal compound, or the porous bead exhibits ion exchange properties, and wherein said properties result in the reversible exchange of lithium and hydrogen ions.
97. A method of extracting lithium from a liquid resource, the method comprising:(a) manufacturing a mixed metal compound, a coated mixed metal compound, or a porous bead as described in any one of claims 1 to 96, wherein the mixed metal compound, the coated mixed metal compound, or the porous bead selectively exchanges lithium ions and protons;(b) contacting the liquid resource to said mixed metal compound, said coated mixed metal compound, or said porous beads to absorb lithium; and(c) contacting an acidic eluent solution to the mixed metal compound, the coated mixed metal compound, or the porous bead to afford a synthetic lithium solution.
98. A mixed metal compound, a coated mixed metal compound, or a porous bead afforded by the method of any one of claims 1-96.
99. A method of extracting lithium from a liquid resource, the method comprising:(a) contacting the liquid resource to the mixed metal compound, the coated mixed metal compound, or the porous bead of claim 98 to absorb lithium; and(b) contacting an acidic eluent to the mixed metal compound, coated mixed metal compound, or porous bead to afford a synthetic lithium solution.
100. A lithium selective sorbent composite comprising a mixed metal compound prepared by the method of any one of claims 1-89, and a binder.
101. A method of extracting lithium from a liquid resource, the method comprising:WSGR Docket No. 50741-727.601(a) contacting the liquid resource to the lithium selective sorbent composite of claim 100 to absorb lithium; and(b) contacting an acidic eluent to the lithium selective sorbent composite to afford a synthetic lithium solution.