Battery cell, battery device, electric device, and energy storage device
By optimizing the particle size distribution and conductive agent combination of the positive electrode film, the internal structure of the battery cell is improved, solving the problems of insufficient battery capacity and cycle performance, and achieving high-capacity and long-life battery performance.
Patent Information
- Application Number
- PCT/CN2025/094369
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-05-12
- Publication Date
- 2026-11-19
AI Technical Summary
Existing technologies cannot simultaneously improve the energy density and cycle performance of individual battery cells, resulting in insufficient battery capacity and lifespan.
By optimizing the particle size distribution of the positive electrode film, controlling the area ratio of large and small particles, and combining carbon nanotubes and conductive carbon black as conductive agents, a hierarchical conductive structure is formed. The contact between the electrode and the current collector is optimized, and the internal structure of the battery is improved by using a porous membrane and a reasonable shell design.
It improves battery capacity and cycle performance, reduces internal resistance and heat generation, extends battery life, and enhances battery dynamic performance and stability.
Smart Images

Figure CN2025094369_19112026_PF_FP_ABST
Abstract
Description
Battery cells, battery packs, electrical devices, and energy storage devices Technical Field
[0001] This application relates to the field of battery cell technology, and in particular to a battery cell, battery device, power supply device, and energy storage device. Background Technology
[0002] In recent years, battery cells have been widely used in energy storage power systems such as hydropower, thermal power, wind power and solar power plants, as well as in many fields such as power tools, electric bicycles, electric motorcycles, electric cars, military equipment, and aerospace.
[0003] With the market's increasing demands for both driving range and cycle life of electrical devices, higher requirements are being placed on the energy density and cycle performance of individual battery cells. However, existing technologies struggle to simultaneously improve these performance characteristics, which has become a pressing technical problem to be solved in this field. Summary of the Invention
[0004] This application is made in view of the above-mentioned problems, and its purpose is to provide a battery cell with high capacity and good cycle performance.
[0005] This application provides a battery cell comprising a stacked cell, the stacked cell including a positive electrode and a negative electrode. The positive electrode includes a positive current collector and a positive electrode film disposed on at least one side of the positive current collector. The positive electrode film includes lithium transition metal phosphate particles, and at least a portion of the surface of the lithium transition metal phosphate particles is provided with carbon material. In a cross-section of the positive electrode film along the thickness direction of the electrode, the area percentage of particles with a diameter greater than or equal to 1 μm is 12%-50%. In a cross-section of the positive electrode film along the thickness direction of the electrode, the area percentage of particles with a diameter greater than 50 nm and less than or equal to 200 nm is 3.0%-15.0%. In a fully discharged state, the compaction density of the positive electrode is 2.3 g / cm³. 3 -2.6g / cm 3 .
[0006] Studies have shown that to effectively improve the compaction density of the electrode, an appropriate amount of particles with a diameter greater than or equal to 1 μm needs to be introduced into the positive electrode film layer. The applicant found that when the area ratio of particles with a diameter greater than or equal to 1 μm in the cross-section along the thickness direction of the positive electrode film layer is less than 12%, or the area ratio of particles with a diameter of 50 nm-200 nm is less than 3%, insufficient particle gradation will occur, limiting the improvement of compaction density and thus preventing an effective increase in battery capacity. When the battery cell is in a fully discharged state, the compaction density of the positive electrode is less than 2.3 g / cm³. 3In such cases, the battery not only struggles to achieve ideal capacity performance, but also suffers from insufficient interparticle connectivity, hindering the formation of electron conduction networks and lithium-ion transport channels, significantly increasing internal resistance. When the area ratio of particles with a diameter of 50nm-200nm in the cross-section of the positive electrode film along the electrode thickness direction exceeds 15%, the excessively high proportion of small particle area leads to increased internal resistance of the positive electrode film, exacerbating heat generation during battery cycling and degrading cycle performance. Conversely, when the area ratio of particles with a diameter greater than or equal to 1μm in the cross-section of the positive electrode film along the electrode thickness direction exceeds 50%, or when the compaction density of the positive electrode sheet of the battery cell in a fully discharged state exceeds 2.6g / cm³, the battery will not achieve the desired capacity performance. 3 When large particles are compressed on the electrode, a significant stress concentration effect will occur, leading to problems such as contact failure between particles, loosening of the film structure, and even shedding of active materials, which will have a negative impact on cycle performance.
[0007] This application improves battery capacity through a combination of stacked cell structure design and optimized particle size distribution of the lithium transition metal phosphate cathode film. Simultaneously, by reducing the area ratio of large particles and controlling the compaction density of the cathode sheet, stress concentration caused by large particles during electrode compaction in the stacked cell is mitigated, effectively alleviating issues of film structure loosening and active material shedding, thus improving battery cycle performance. Further controlling the area ratio of small particles within a suitable range ensures sufficient particle filling while avoiding excessive small particles that could increase the resistance of the cathode film, reducing heat generation during cycling, and improving battery kinetic and cycle performance. Through the synergistic design of the stacked cell and cathode sheet, the battery's capacity, cycle performance, and kinetic performance are improved.
[0008] In any embodiment, in the cross-section of the positive electrode film layer along the thickness direction of the electrode sheet, the area ratio of particles with a diameter greater than or equal to 1 μm and less than or equal to 5 μm is 12%-50%.
[0009] When the area ratio of particles with a diameter greater than or equal to 1 μm and less than or equal to 5 μm in the cross-section of the positive electrode film along the thickness direction of the electrode sheet is within the above range, it is beneficial to further improve the phenomenon of film loosening and active material shedding caused by stress concentration when large particles are pressed into the electrode sheet, thereby improving the cycle performance of the battery while maintaining high capacity.
[0010] In any embodiment, in the cross-section of the positive electrode film layer along the electrode thickness direction, the area ratio of particles with a particle size greater than or equal to 1 μm and less than or equal to 5 μm is 12%-40%.
[0011] When the area ratio of particles with a diameter greater than or equal to 1 μm and less than or equal to 5 μm in the cross-section of the positive electrode film along the thickness direction of the electrode sheet is within the above range, it is beneficial to further improve the phenomenon of film loosening and active material shedding caused by stress concentration when large particles are pressed into the electrode sheet, while maintaining high capacity, and further improve the cycle performance of the battery.
[0012] In any embodiment, the uniformity of particle distribution with a diameter greater than or equal to 1 μm in the cross-section of the positive electrode film layer along the electrode thickness direction is 0.2%-5%, and can be selected as 0.2%-2%.
[0013] The uniformity of the distribution of particles with a diameter greater than or equal to 1 μm in the cross-section along the thickness direction of the positive electrode film is within a suitable range. The uniformly distributed large particles can effectively reduce the stress concentration in local areas of the film, so that the stress during the film compaction process can be uniformly dispersed throughout the entire area of the film, avoiding the local stress concentration caused by particle agglomeration, reducing the probability of film peeling, and improving the cycle performance of the battery.
[0014] In any embodiment, in the cross-section of the positive electrode film along the electrode thickness direction, the median L of the spheroidality in the cumulative distribution curve of the spheroidality area of particles with a diameter greater than or equal to 1 μm is... A50 It is 0.6-0.8.
[0015] The median sphericity of particles with a diameter of 1 μm or greater is within the above range. Larger particles have better sphericity, which reduces particle bridging caused by the irregular shape of large particles, reduces the void content in the electrode, and at the same time reduces the stress concentration aggravated by the irregularity of large particles. This improves the phenomenon of film loosening and active material shedding, and the battery cell has high capacity and good cycle performance.
[0016] In any embodiment, in the cross-section of the positive electrode film along the electrode thickness direction, the median L of the spheroidality in the cumulative distribution curve of the spheroidality area of particles with a diameter greater than or equal to 1 μm is... A50 It is 0.65-0.75.
[0017] The median sphericity of particles with a diameter of 1 μm or greater is within the above range, which helps to reduce stress concentration caused by the irregularity of large particles exacerbating electrode pressure, and improves the phenomenon of film loosening and active material shedding.
[0018] In any embodiment, in the cross-section of the positive electrode film along the electrode thickness direction, the median L of the spheroidality in the cumulative distribution curve of the spheroidality area of particles with a diameter greater than or equal to 1 μm is... A50 It is 0.67-0.75.
[0019] The median sphericity of particles with a diameter of 1 μm or greater is within the above range, which can further improve the stress concentration that occurs when large particles are pressed into the electrode, reduce the probability of film loosening and active material shedding, and improve the cycle life of the battery cell.
[0020] In any embodiment, in the cross-section of the positive electrode film layer along the thickness direction of the electrode sheet, the area ratio of particles with a diameter greater than 50 nm and less than or equal to 200 nm is 5.0%-15.0%.
[0021] The area ratio of particles with a diameter greater than 50nm and less than or equal to 200nm is within the above range. The positive electrode film layer has an appropriate amount of small particles, which ensures sufficient particle filling degree, while avoiding the adverse effect of excessive small particle area ratio on the film layer resistance. The battery improves the dynamic performance of the battery while having good capacity.
[0022] In any embodiment, in the cross-section of the positive electrode film layer along the thickness direction of the electrode sheet, the area ratio of particles with a diameter greater than 50 nm and less than or equal to 200 nm is 5.0%-10.0%.
[0023] When the area ratio of particles with a diameter greater than 50nm and less than or equal to 200nm is within the above range, the positive electrode film has a good particle size distribution, which further reduces the resistivity of the positive electrode film and further improves the dynamic performance of the battery on the basis of good capacity.
[0024] In any embodiment, the thickness of the positive electrode film on one side is 70 μm-120 μm.
[0025] The specific capacity of lithium-containing transition metal phosphate particles is relatively low. Studies have shown that when the single-sided thickness of the positive electrode film is less than 70 μm, the battery capacity is difficult to meet market demand. A single-sided thickness of the positive electrode film within the aforementioned range is beneficial for improving the capacity of individual battery cells.
[0026] In any embodiment, the thickness of the positive electrode film on one side is 90 μm-120 μm.
[0027] A single-sided thickness of the positive electrode film within the above-mentioned range is beneficial for further improving the capacity of the battery cell.
[0028] In any embodiment, the thickness of the positive electrode film on one side is 100μm-120μm.
[0029] Increasing the thickness of the positive electrode film on one side is beneficial to improving the battery capacity. The applicant found that when the thickness of the positive electrode film on one side is greater than or equal to 100 μm, the positive electrode film is more prone to loosening and shedding of active material. The embodiments of this application reduce the area ratio of large particles and reduce the compaction density of the positive electrode film, which together improves the stress concentration phenomenon of large particles in the stacked cell during electrode compaction. At the same time, an appropriate amount of small particles are added so that the electrode can still have a good compaction density while giving up a certain amount of large particles, and the battery has a good capacity and cycle performance.
[0030] In any embodiment, the positive electrode film layer further includes a conductive agent, and the total area of the agglomerated region of the conductive agent accounts for 0.2%-6%, optionally 1.5%-5%, based on the total area of the cross-section of the positive electrode film layer along the thickness direction of the electrode sheet.
[0031] Based on the total area of the cross-section along the thickness direction of the positive electrode film, the total area ratio of the agglomeration region of the conductive agent within the above range indicates that the conductive agent in the positive electrode film is uniformly dispersed and easily forms a uniform conductive network, which is beneficial to reducing local polarization and even lithium plating problems generated during battery cycling.
[0032] Meanwhile, the appropriate amount of small particles in this application can serve as a basic conductive framework to fill the gaps between large particles, while the dispersed conductive agent agglomerates serve as long-range conductive nodes, forming a hierarchical conductive structure. Since large particles in lithium transition metal phosphate particles are prone to rebound, the agglomeration area of the conductive agent within the above-mentioned range can also suppress the rebound of large particles by means of the uniform distribution of the conductive agent, forming mechanical constraints on the particles and even the film layer, improving the cohesion of the film layer, reducing the phenomenon of film layer powder shedding and active material shedding, and improving the cycle life of the battery.
[0033] In any embodiment, the conductive agent includes carbon nanotubes, which include one or more of single-walled carbon nanotubes, few-walled carbon nanotubes, and multi-walled carbon nanotubes. Optionally, the conductive agent also includes conductive carbon black.
[0034] Carbon nanotubes have a high aspect ratio, which is beneficial for bridging particles of different sizes in the thickness direction through their unique fiber structure. This forms a long-range conductive path while increasing the binding force between particles, reducing local polarization and even lithium plating problems during battery cycling, and improving the cycle life of the battery. Furthermore, through the binding effect, it can reduce the rebound phenomenon of large particles in the positive electrode film and reduce the shedding of active materials in the film.
[0035] Conductive carbon black has a small size, adheres to the surface of positive electrode particles and fills the gaps between the positive electrode particles, forming dense point-shaped conductive contacts. When used in combination with carbon nanotubes, both long-range and short-range conductivity are achieved, which is conducive to further optimizing the conductive network in the positive electrode film layer. Meanwhile, the conductive agent has a large specific surface area, which facilitates electrolyte absorption and retention, can reduce the extrusion of electrolyte caused by a high increase rate of expansion force of the electrode plate during long cycles, and improves the long-cycle life of the battery.
[0036] In any embodiment, the agglomerated region of the conductive agent includes carbon nanotubes and conductive carbon black.
[0037] Researchers have found that carbon nanotubes are prone to agglomeration due to their high surface energy, which results in uneven dispersion in the positive electrode film layer and prevents the formation of an effective carbon nanotube network structure. Conductive carbon black and carbon nanotubes have relatively close surface energies, and can adsorb on the surface of carbon nanotubes to form a physical barrier, increase the resistance to agglomeration of carbon nanotubes, reduce direct contact between carbon nanotubes, thereby inhibiting the agglomeration phenomenon and improving the distribution uniformity of carbon nanotubes in the positive electrode film layer. On the one hand, this helps improve the conductivity of the positive electrode film layer and enhance the kinetic performance of the battery; on the other hand, it helps exert the binding effect of carbon nanotubes on the positive electrode film layer, reduce the risk of the positive electrode film layer peeling off, and further improve the kinetic performance and cycle life of the battery. In addition, the agglomeration of carbon nanotubes in the agglomerated region of the conductive agent will also cause local blockage of ion transport pathways in the agglomerated region of the conductive agent. The matching use of conductive carbon black can improve the lithium ion transport capacity in this region, reduce local polarization, and further improve the cycle stability of the battery.
[0038] In any embodiment, based on the mass of the positive electrode film layer, the mass content C1 of the carbon nanotubes satisfies: 0<C1≤2.5%, and the mass content C2 of the conductive carbon black satisfies: 0<C2≤2.5%.
[0039] When the mass contents of carbon nanotubes and conductive carbon black are within the above ranges, the agglomeration phenomenon of carbon nanotubes can be effectively alleviated and a good conductive network structure can be formed, so as to effectively reduce the stress concentration of the positive electrode film layer, increase the liquid retention rate of the positive electrode film layer during long cycles, further reduce the risk of peeling of the electrode plate film layer and the degree of polarization, improve the kinetic performance of the battery and improve the cycle life of the battery.
[0040] In any embodiment, the positive electrode film layer further includes a dispersant, and the dispersant includes hydrogenated nitrile butadiene rubber (HNBR).
[0041] The polar groups (such as cyano, -CN) in hydrogenated nitrile butadiene rubber (HNBR) molecules can interact with hydroxyl groups (-OH) or metal oxide sites on the surface of lithium transition metal phosphate particles (such as hydrogen bonding, dipole interaction), enhancing the compatibility between particles and solvents, reducing the interfacial tension between particles and solvents, and improving the interfacial tension of large particles more significantly. This makes it easier for large and small particles in the film to be evenly dispersed, reducing particle aggregation caused by hydrophobicity, improving the dispersibility of large particles in the positive electrode film, and reducing stress concentration generated during the film die-cutting process.
[0042] Meanwhile, during the drying and film formation of the slurry, the elastic network structure of HNBR can buffer the shrinkage stress caused by solvent evaporation, reduce the re-aggregation of conductive agents due to capillary forces during this process, reduce the area ratio of conductive agent agglomeration regions, and the uniform distribution of conductive agents helps to suppress the rebound of large particles, forming mechanical constraints on particles and even film layers, improving the cohesive force of film layers, reducing film layer powder shedding and active material shedding, and improving the cycle life of the battery.
[0043] In any embodiment, based on the mass of the positive electrode film, the mass content of the dispersant is 0.5%-2%.
[0044] When the mass content of the dispersant is within the above range, it can achieve uniform dispersion of particles in the positive electrode film while maintaining a high loading capacity, resulting in good capacity and cycle performance of the battery.
[0045] In any embodiment, the positive electrode film layer has a base coating layer in the bottom region near the positive electrode current collector. The base coating layer includes a conductive agent and a binder. The conductive agent includes carbon nanotubes and conductive carbon black, and the binder includes vinylidene fluoride polymer.
[0046] In any embodiment, the positive electrode film layer has a base coating layer in the bottom region near the positive electrode current collector, and the thickness of the base coating layer is 0.5μm-5μm.
[0047] The undercoating layer provided in this application helps improve the adhesion between the positive electrode film and the positive electrode current collector and alleviates stress concentration at large particles, thereby reducing the probability of positive electrode film detachment and improving the cycle stability of the battery. Simultaneously, compared to direct contact between the positive electrode current collector and the positive electrode film, the increased contact area between the undercoating layer and the positive electrode film helps increase the area for electron transport between the current collector and the positive electrode film, thereby reducing the internal resistance of the electrode and improving the battery's dynamic performance.
[0048] In any embodiment, the median C of the graphitization degree C value in the cumulative distribution curve of the positive electrode film obtained in the laser microscopy confocal Raman spectroscopy instrument scanning mode is... 50 Greater than or equal to 0.95 and less than or equal to 1.20; wherein, the degree of graphitization C is I. G / ID I G This indicates that the Raman spectrum is at 1580±100 cm⁻¹ -1 The intensity of peak G at I D This indicates that the Raman spectrum is at 1350±100 cm⁻¹ -1 The intensity of peak D at that location.
[0049] In the cumulative distribution curve of graphitization degree C obtained by laser microscopy confocal Raman spectroscopy in instrument scanning mode, the median C of graphitization degree is... 50 Within the aforementioned range, the compaction density of the electrode can be further improved by relying on particle slippage, without overly relying on the ratio of large to small particles in the positive electrode film. This ensures that the area ratio of large and small particles is within a suitable range, which helps reduce the probability of positive electrode film shedding and avoids excessive resistance of the positive electrode film. This helps improve the cycle performance and dynamic performance of the battery while maintaining its capacity.
[0050] In any embodiment, the lithium transition metal phosphate particles in the positive electrode film layer comprise components represented by the following general formula: Li m Fe x P y O j Q q Formula I, wherein Q includes one or more of Al, Na, K, Mg, Cu, Mn, Cr, Zn, Pb, Ca, Co, Ni, Sr, Nb, V, Ti, B, S, Si, N, F, Cl, and Br, with 0.8≤m≤1.15, 0.9≤x≤1, 0.95≤y≤1, 3.5≤j≤4, and 0≤q≤0.1.
[0051] In any embodiment, the lithium transition metal phosphate particles include titanium, and the mass content of titanium is 500ppm-8000ppm, optionally 1000ppm-3000ppm, based on the total mass of the lithium transition metal phosphate particles in the positive electrode film.
[0052] When titanium is doped into lithium-containing transition metal phosphate particles, the Ti-OP bonds formed have a strong bonding effect. By anchoring phosphate groups, the contraction / expansion of the lattice during lithium ion insertion / extraction is reduced, thereby suppressing the structural stress caused by phase transition and improving the cycle life of the battery. In addition, the Ti-OP bonds can provide a more stable channel for lithium ion diffusion, reduce the migration energy barrier, and improve the kinetic performance of the battery.
[0053] Within the above-mentioned range, the mass content of titanium is beneficial to improving the lithium-ion transport rate of the positive electrode active material, reducing the risk of lithium plating, and improving the kinetic performance of the battery.
[0054] In any embodiment, the lithium transition metal phosphate particles include vanadium, and the mass content of vanadium is 500ppm-5000ppm, optionally 500ppm-3000ppm, based on the total mass of the lithium transition metal phosphate particles in the positive electrode film.
[0055] When vanadium is doped into lithium-containing transition metal phosphate particles, it exhibits multi-valence characteristics. When +5 vanadium (V5+) is doped into phosphorus sites, its larger radius introduces lattice distortion, expands lithium-ion diffusion channels, and improves the ionic conductivity of the cathode active material. When +3 vanadium (V3) is doped into transition metal sites, it compensates for the charge through lithium vacancies or interstitial oxygen, forming defect energy levels and improving the electronic conductivity of the cathode active material.
[0056] Vanadium content within the above range is beneficial for improving the lithium-ion transport rate of the cathode active material, enhancing its electronic conductivity, and further improving the battery's kinetic performance through synergistic effects with titanium doping.
[0057] In any embodiment, the porosity of the positive electrode film is 14%-28%.
[0058] A porosity within the above-mentioned range in the positive electrode film indicates a better particle size distribution in the positive electrode film, which is beneficial for improving the electrolyte retention characteristics, improving the ion diffusion of the positive electrode film with a certain area ratio of large particles, and improving the kinetic performance of the battery.
[0059] In any embodiment, the resistivity of the positive electrode film is 10 Ω·cm-35 Ω·cm.
[0060] When the resistivity of the positive electrode film is within a suitable range, it is beneficial to reduce electron transport impedance, reduce charge and discharge polarization, and improve the dynamic performance of the battery.
[0061] In any embodiment, the battery cell further includes a separator disposed between the positive electrode and the negative electrode. The separator includes a base film, ceramic layers disposed on both sides of the base film, and an adhesive layer disposed on at least one side of the ceramic layer away from the base film. The adhesive layer is a continuous layer with a porous structure and includes a vinylidene fluoride polymer.
[0062] The separator provided in this application uses a continuous porous layer as the adhesive layer, which has a larger bonding area compared to the island-shaped adhesive layer in the prior art. This results in a stronger and more uniform bond between the separator and the positive electrode film. Simultaneously, the porous structure in the adhesive layer allows for both lithium-ion transport efficiency and improved battery dynamics. Furthermore, compared to wound cells, stacked cells experience less clamping force between the electrodes during cell fabrication. Lithium-containing transition metal phosphate particles with a diameter greater than or equal to 1 μm can reduce the compactness of the internal components during rebound, increasing cell impedance and the probability of film shedding or even detachment. The separator provided in this application, using a continuous porous layer as the adhesive layer, is particularly suitable for stacked cells, improving the rebound phenomenon during long-cycle operation and enhancing battery capacity retention over extended periods.
[0063] This application embodiment uses a continuous layer with a porous structure as an adhesive layer to improve the adhesion between the separator and the electrode while maintaining the air permeability and porosity of the separator, thereby improving the stability of the electrode and further reducing the risk of powder shedding or even internal short circuit due to relative displacement between the electrode and the separator, thus improving the cycle stability of the battery.
[0064] In any embodiment, the battery cell includes a housing, and the stacked cells are housed within the housing. The housing has a length dimension of L0, a width dimension of W0, and a thickness dimension of H0, with 450mm≤L0≤1300mm, 100mm≤W0≤150mm, and 14mm≤H0≤22mm.
[0065] The casing size of the battery cell in this embodiment is within the above-mentioned range, which is beneficial for the battery to achieve a better capacity.
[0066] In any embodiment, the length dimension L0 of the housing satisfies: 450mm≤L0≤650mm.
[0067] When the length dimension L0 of the casing satisfies 450mm≤L0≤650mm, the battery cell has a shorter length, which is beneficial to shorten the electron transport path, reduce the internal resistance of the battery, reduce the wetting distance of the electrolyte in the electrode pores, improve the wetting uniformity, and improve the dynamic performance of the battery. Especially under fast charging conditions, it can reduce the phenomenon of uneven temperature rise and uneven current density in the length direction of the electrode.
[0068] In any embodiment, the length dimension L0 of the housing satisfies: 900mm≤L0≤1300mm.
[0069] When the length dimension L0 of the casing satisfies 900mm≤L0≤1300mm, the significantly increased single-cell size can effectively simplify the traditional module structure, enabling the single cell to be directly integrated into the battery pack. The battery is fixed by structural components set at the end of the large surface, significantly improving space utilization. This increases the overall capacity of the battery system within the same volume, while reducing the number of structural components and improving battery energy density.
[0070] In any embodiment, the shell material is a soft-pack material, which includes an aluminum-plastic composite film. Optionally, it includes one or more of polypropylene (PP), polybutylene terephthalate (PBT), polybutylene succinate (PBS), nylon, polyethylene terephthalate (PET), and polyethylene (PE) forming a composite film with aluminum.
[0071] Pouch cells possess high elongation, resulting in thin, flexible casings that improve space utilization and thus energy density. However, pouch cells, such as aluminum-plastic composite films, have poor thermal conductivity, leading to lower heat dissipation efficiency. Therefore, excessively high particle area in the positive electrode film increases resistivity, causing excessive heat generation during cycling and exacerbating the heat dissipation problem. This application addresses this issue by using pouch cells as the casing and controlling the particle area ratio in the positive electrode film within a suitable range, resulting in high capacity and good cycle performance.
[0072] In any embodiment, the housing includes a first sealing area, which is disposed at at least one end of the laminated cell extending in the width direction; the first sealing area includes a folded edge structure extending in the length direction, on which encapsulating adhesive is disposed, and the encapsulating adhesive is continuously disposed in the length direction and fixes the folded edge structure.
[0073] This application embodiment further enhances the sealing strength of the first sealing area by including a folded edge structure extending along the length direction. The continuous arrangement of the encapsulating adhesive along the length direction and the fixing of the folded edge structure, compared to a discontinuous arrangement of the encapsulating adhesive along the length direction, further improves the sealing strength, achieving continuous reinforcement of the sealing area along its length and reducing the probability of the electrode breaking open the sealing area in the packaging during cycling.
[0074] In any embodiment, the housing includes at least one second sealing area, the second sealing area being disposed at at least one end of the laminated cell extending along the length direction of the housing, the second sealing area being disposed on the tab side of the laminated cell.
[0075] The second sealing area is located on the tab side. The tab needs to be connected to the lead-out component. The connection strength between the lead-out component and the shell material is relatively weak, which makes it easy for gas to escape from the second sealing area. This is conducive to directional pressure relief of the battery, reducing the impact on adjacent cells during thermal runaway, and improving the overall service life of the battery.
[0076] In any embodiment, the outer periphery of the laminated cell is provided with a plurality of rubber rings that surround in the width direction, and the rubber rings that surround in the width direction are spaced apart in the length direction.
[0077] The rubber rings that wrap around the width of the cell and are spaced apart along the length help to fix the position between the electrodes in the cell, reducing the probability of cell displacement during battery shaking. This is especially suitable for batteries with a large length, as it can effectively reduce the mutual displacement between the electrodes in the length direction, thus reducing lithium plating. This helps to maintain the stability of the internal spatial structure of the battery, thereby not affecting the normal operation of the battery.
[0078] In any embodiment, at 25°C, the capacity of the battery cell is 100Ah-300Ah, optionally 110Ah-190Ah, and further optionally 125Ah-180Ah.
[0079] The battery cell in this application embodiment uses a suitable housing size to accommodate the stacked cells, and controls the proportion of large particles in the film layer of the positive electrode in the stacked cells to be reasonable, so that the battery cell has a high capacity.
[0080] A second aspect of this application provides a battery device, including the battery cell provided in the first aspect of this application.
[0081] A third aspect of this application provides an electrical device, which includes the battery device provided in the second aspect, the battery device being used to provide electrical energy.
[0082] The fourth aspect of this application provides an energy storage device, which includes the battery device provided in the second aspect, the battery device being used to store electrical energy. Attached Figure Description
[0083] Figure 1 is a schematic diagram of a diaphragm according to an embodiment of this application;
[0084] Figure 2 is a schematic diagram of a diaphragm in the prior art;
[0085] Figure 3 is a schematic diagram of the surface morphology of the adhesive layer of the diaphragm according to an embodiment of this application;
[0086] Figure 4 is a front view of a battery cell according to an embodiment of this application;
[0087] Figure 5 is a schematic diagram of an electrical device according to an embodiment of this application.
[0088] Explanation of reference numerals in the attached drawings: 20 separator; 201 base film; 202 ceramic layer; 203 adhesive layer; 5 battery cell; 50 casing; 51 first sealing area; 52 second sealing area; 53 lead-out component; X length direction; Y width direction; Z thickness direction. Detailed Implementation
[0089] The following detailed description, with appropriate reference to the accompanying drawings, specifically discloses embodiments of the battery cell, battery device, power consumption device, and energy storage device of this application. However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repetitive descriptions of practically identical structures may be omitted. This is to avoid unnecessarily lengthy descriptions and to facilitate understanding by those skilled in the art. Furthermore, the accompanying drawings and the following description are provided for the purpose of enabling those skilled in the art to fully understand this application and are not intended to limit the subject matter of the claims.
[0090] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values of 1 and 2 are listed, and if maximum range values of 3, 4, and 5 are listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0091] Unless otherwise specified, all embodiments and optional embodiments of this application may be combined with each other to form new technical solutions, and such technical solutions should be considered to be included in the disclosure of this application.
[0092] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions, and such technical solutions shall be deemed to be included in the disclosure of this application.
[0093] Unless otherwise specified, all steps in this application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the method may also include step (c), indicating that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.
[0094] In this application, the terms "multiple" or "various" refer to two or more kinds of things.
[0095] Unless otherwise stated, the terms used in this application have the common meanings as commonly understood by those skilled in the art.
[0096] Unless otherwise stated, the values of the parameters mentioned in this application can be determined using various testing methods commonly used in the art, for example, according to the testing methods given in the embodiments of this application. Unless otherwise stated, the test temperature for each parameter is 25°C.
[0097] In embodiments of this application, the battery device may include one or more battery cell assemblies for providing voltage and capacity. A battery cell assembly may include multiple pouch cell batteries connected in series, parallel, or a combination of these pouch cell batteries via a busbar. For example, a battery cell assembly is typically formed by arranging multiple pouch cell batteries; a battery cell assembly may also be a battery module, which is formed by arranging and fixing multiple pouch cell batteries into a single module. As an example, a battery module may be formed by bundling multiple battery cells together with cable ties.
[0098] The battery device can be a battery pack, which includes a housing and one or more individual battery cells housed within the housing. The individual battery cells can be battery modules, which can be housed within the housing by fixing the battery modules to the housing; alternatively, multiple pouch battery cells can be directly fixed to the housing and housed within the housing.
[0099] In embodiments of this application, the housing may include a first housing and a second housing. The first housing and the second housing are fastened together to form a closed space inside the housing for housing individual battery cells. Here, "closed" refers to covering or shutting down; it can be sealed or unsealed. The first housing may be a top cover or a bottom plate. For example, the housing may include a top cover, a frame, and a bottom plate. The top cover and the bottom plate are respectively connected to the frame, forming a closed space inside the housing for housing individual battery cells.
[0100] In embodiments of this application, the housing can be part of the vehicle's chassis structure. For example, a portion of the housing can be at least a part of the vehicle's floor, or a portion of the housing can be at least a part of the vehicle's crossbeams and longitudinal beams.
[0101] In this embodiment, the battery cell can be a rechargeable battery, which refers to a battery cell that can be recharged after discharge to activate the active materials and continue to be used; the battery cell can be a lithium-ion battery. The battery cell can be flat.
[0102] The battery mentioned in the embodiments of this application can be a single physical module comprising one or more battery cells to provide higher voltage and capacity. For example, the battery mentioned in this application can include battery cells, battery modules, or battery packs.
[0103] A single battery cell is the smallest unit that makes up a battery, capable of charging and discharging independently. When there are multiple battery cells, they are connected in series, parallel, or a combination of both via a busbar. In some embodiments, the battery can be a battery module; when there are multiple battery cells, they are arranged and fixed to form a battery module. In some embodiments, the battery can be a battery pack, comprising a housing and battery cells, with the battery cells or battery modules housed within the housing. In some embodiments, the housing can be part of the vehicle's chassis structure. For example, a portion of the housing can be at least part of the vehicle's floor, or a portion of the housing can be at least part of the vehicle's crossbeams and longitudinal beams.
[0104] In some implementations, the battery can be an energy storage device. Energy storage devices include energy storage containers, energy storage cabinets, etc.
[0105] In some embodiments, individual battery cells can be assembled into battery modules, and the number of battery cells contained in a battery module can be multiple, with the specific number adjustable according to the application and capacity of the battery module. In some embodiments, the above-mentioned battery modules can also be assembled into battery packs, and the number of battery modules contained in the battery packs can be adjusted according to the application and capacity of the battery packs.
[0106] A single battery cell includes electrode components and an electrolyte.
[0107] Electrode assemblies typically include positive and negative electrodes. The negative electrode is the electrode that absorbs or lithiates lithium ions during charging and releases or delithiates lithium during discharging. The positive electrode is the electrode that absorbs or delithiates lithium ions during charging and absorbs or lithiates lithium during discharging.
[0108] Lithium-containing transition metal phosphate materials offer significant advantages over lithium-containing transition metal oxide materials, including higher safety performance, longer cycle life, lower raw material costs, and superior high-temperature stability. However, these materials also have inherent drawbacks, particularly their lower theoretical specific capacity, which severely restricts the improvement of battery capacity. The applicant's research found that stacked cells, compared to wound cells, do not have corner areas, resulting in higher space utilization within the battery. Using stacked cells helps improve the volumetric energy density of the battery. Furthermore, increasing the content of large and small particles to optimize the particle size distribution of the positive electrode active material can further improve the compaction density of the electrode, thereby increasing the volumetric energy density of the battery. However, during electrode compaction, stress concentration easily occurs at large particles, leading to interparticle contact failure, loosening of the film structure, and even shedding of active material. While small particles can fill gaps and further improve the compaction density of the electrode, excessive small particles increase the resistance of the positive electrode film. Because stacked cells lack the constraint of corner areas, they lack radial binding forces, making them more prone to stress concentration caused by large particles, which can lead to film shedding in the electrodes. Film shedding results in reduced battery capacity, internal micro-short circuits, and exacerbated electrolyte side reactions, adversely affecting battery performance. Obtaining batteries with good capacity, cycle performance, and kinetic performance is a pressing technical problem that needs to be solved in this field.
[0109] The first aspect of this application provides a battery cell, including a stacked cell, comprising a positive electrode and a negative electrode. The positive electrode includes a positive current collector and a positive electrode film disposed on at least one side of the positive current collector. The positive electrode film includes lithium transition metal phosphate particles, and at least a portion of the surface of the lithium transition metal phosphate particles is provided with carbon material. In a cross-section of the positive electrode film along the thickness direction of the electrode, the area percentage of particles with a diameter greater than or equal to 1 μm is 12%-50%. In a cross-section of the positive electrode film along the thickness direction of the electrode, the area percentage of particles with a diameter of 50 nm-200 nm is 3.0%-15.0%. In a fully discharged state, the compaction density of the positive electrode is 2.3 g / cm³. 3 -2.6g / cm 3 .
[0110] Studies have shown that to effectively improve the compaction density of the electrode, it is necessary to introduce an appropriate amount of particles with a diameter greater than or equal to 1 μm into the positive electrode film layer. The applicant discovered that the loss in electrode compaction density caused by the reduction in the content of large particles can be compensated for by adding an appropriate amount of small particles. When the area ratio of particles with a diameter greater than or equal to 1 μm in the cross-section along the thickness direction of the positive electrode film layer is less than 12%, or the area ratio of particles with a diameter of 50 nm-200 nm is less than 3%, insufficient particle gradation will result, limiting the improvement in compaction density and thus preventing an effective increase in battery capacity. When the battery cell is in a fully discharged state, the compaction density of the positive electrode is less than 2.3 g / cm³. 3In such cases, the battery not only struggles to achieve ideal capacity performance, but also suffers from insufficient interparticle connectivity, hindering the formation of electron conduction networks and lithium-ion transport channels, significantly increasing internal resistance. When the area ratio of particles with a diameter of 50nm-200nm in the cross-section of the positive electrode film along the electrode thickness direction exceeds 15%, the excessively high proportion of small particle area leads to increased internal resistance of the positive electrode film, exacerbating heat generation during battery cycling and degrading cycle performance. Conversely, when the area ratio of particles with a diameter greater than or equal to 1μm in the cross-section of the positive electrode film along the electrode thickness direction exceeds 50%, or when the compaction density of the positive electrode sheet of the battery cell in a fully discharged state exceeds 2.6g / cm³, the battery will not achieve the desired capacity performance. 3 When large particles are compressed on the electrode, a significant stress concentration effect will occur, leading to problems such as contact failure between particles, loosening of the film structure, and even shedding of active materials, which will have a negative impact on cycle performance.
[0111] This application improves battery capacity through a combination of stacked cell structure design and optimized particle size distribution of the lithium transition metal phosphate cathode film. Simultaneously, by reducing the area ratio of large particles and controlling the compaction density of the cathode sheet, stress concentration caused by large particles during electrode compaction in the stacked cell is mitigated, effectively alleviating issues of film structure loosening and active material shedding, thus improving battery cycle performance. Further controlling the area ratio of small particles within a suitable range ensures sufficient particle filling while avoiding excessive small particles that could increase the resistance of the cathode film, reducing heat generation during cycling, and improving battery kinetic and cycle performance. Through the synergistic design of the stacked cell and cathode sheet, the battery's capacity, cycle performance, and kinetic performance are improved.
[0112] In this application, a laminated cell refers to a cell formed by stacking a positive electrode, a separator, and a negative electrode together.
[0113] Lithium-containing transition metal phosphate particles refer to phosphate materials containing lithium and transition metal elements, and can be detected by any method known in the art. For example, they can be detected by combining X-ray diffraction (XRD) with energy dispersive spectroscopy (EDS) or inductively coupled plasma mass spectrometry (ICP-MS).
[0114] It should be noted that the positive electrode film layer contains lithium transition metal phosphate particles, but the positive electrode film layer does not only refer to the positive electrode active material layer. Other film layers that are connected to the positive electrode active material layer and are difficult to distinguish, such as the undercoat layer and the liquid retention layer, are all collectively referred to as the positive electrode film layer.
[0115] In this application, the term "particle" refers to a particle in the positive electrode film layer that has a recognizable complete boundary in the field of view at a certain magnification, such as 10,000x. Defects and scratches may exist inside the particle, but a complete boundary sufficient to divide the particle cannot be identified inside the particle.
[0116] The particle identification method is as follows: The positive electrode film layer is cut along the thickness direction of the electrode sheet using an argon ion beam (for example, a Leica EM TIC 3X CP device can be used, operating voltage: 6kV, operating time: 6h). After exposing the cut surface, a scanning electron microscope (SEM) is used (for example, a Hitachi SU8230 device can be used, operating voltage: 3kV, beam current: high, probe model: U (LA100), working distance <5mm) to observe the cut surface along the thickness direction of the electrode sheet. Images are acquired using a field emission scanning electron microscope at a non-edge location in the cut surface of the positive electrode film layer (after observing the electrode edge under the SEM, the field of view is adjusted to the center of the sample) in secondary electron mode. Electron micrographs are taken at 10kx magnification, and the particles in the electron micrographs are analyzed using ImageJ software (1.46r, win64 version). The specific steps for using ImageJ software are as follows: Load the scanning electron microscope (SEM) image to be analyzed; use the Cellpose plugin to identify particles, and then perform manual corrections; use ImageJ to read and analyze data. The specific method for using the Cellpose plugin to identify particles is as follows: Set the segmentation diameter parameter (diameter in the Segmentation module) to 15 pixels, click "run cyto3" to identify particles; manually mark particles in the image that were not identified by the software, were not fully identified, or were identified incorrectly. Particles that were not identified by the software, were not fully identified, or were identified incorrectly mainly include the following: 1. Particles that are too large or have scratches on their surface, making them unidentifiable or incompletely identifiable; 2. During argon ion beam cutting, scratches may be generated on the particle surface, and the software may misinterpret these scratches as particle boundaries, leading to identification errors; 3. Particles that are too small and were not successfully identified; 4. Particles located at the edge of the SEM field of view, with the particle's interior penetrated by the edge, preventing a complete view of the morphology, resulting in identification errors due to partial identification replacing the whole.For the unidentified or misidentified particles mentioned above, manual calibration is performed. The specific process is as follows: 1. Delete large particles located around the edges of the scanning electron microscope that are not fully displayed. 2. Determine if any unidentified or misidentified particles have internal cracks or scratches. If no cracks or scratches are found, classify it as a single particle and manually mark it based on the observed particle boundary. 3. If cracks or scratches are found inside the particle, determine if they penetrate the particle. If not, classify it as a single particle and manually mark it. 4. If cracks or scratches penetrate the particle, determine if they are linear or irregular. 5. If the cracks or scratches are irregular, classify them as the boundary between particles and divide the particles along this boundary. 6. If the cracks or scratches are linear, perform contrast comparison. 7. If the contrast is not obvious and there is no crack-like appearance, classify it as a scratch and mark it as a single particle. 8. If the contrast is strong and there is a crack-like appearance, classify it as the boundary between particles and mark it as two particles. After manual marking, delete information irrelevant to the particles from the automatic image processing, thus completing the particle identification and marking in the image.
[0117] In the cross-section of the positive electrode film along the thickness direction of the electrode sheet, the area ratio of particles with a diameter greater than or equal to 1 μm can intuitively reflect the ratio of the area of some particles in that particle size range to the total area of the particles, and reflect the size of the particles in that particle size range.
[0118] It is understandable that particles larger than 50 nm, especially in the cross-section of the positive electrode film along the electrode thickness direction, mainly originate from the positive electrode active material. Therefore, the embodiments of this application can accurately and objectively reflect the distribution of lithium transition metal phosphate particles within the positive electrode film by observing and statistically analyzing the particle area in the cross-section of the positive electrode film along the electrode thickness direction.
[0119] In existing technologies, laser particle size analyzers are typically used to statistically analyze the particle size of positive electrode active materials using Malvern laser diffraction. However, the applicant's research indicates that because lithium-containing transition metal phosphate particles are prone to agglomeration, the test results obtained by Malvern laser diffraction based on the principle of laser scattering often only reflect the particle size of the agglomerates, and cannot accurately reflect the particle size of the positive electrode active material, let alone its dispersion state in the film layer. This is because the dispersion of the positive electrode active material in the film layer increases during slurry preparation and film forming rolling. The test results obtained by Malvern laser diffraction are affected by the particle size, specific surface area, and degree of agglomeration of the positive electrode active material. Compared to the actual dispersion in the electrode sheet, the number of large particles obtained by this test is lower than the actual value, and the number of small particles is higher than the actual value. Therefore, the particle size obtained by Malvern laser diffraction cannot be equated with or analogized to the particle size statistically obtained in the embodiments of this application.
[0120] The specific method for testing the area ratio of particles with a diameter greater than or equal to 1 μm in the cross-section of the positive electrode film along the electrode thickness direction is as follows: Particles in the cross-section of the positive electrode film along the electrode thickness direction are identified according to the method described above in this application. The images after particle identification and labeling are imported into ImageJ software for analysis. The scale is set based on the scanning electron microscope image. The particle size, area, sphericity, and roughness of the particles in the cross-section along the electrode thickness direction are statistically analyzed using the "Feret," "Area," "Round," and "Solidity" analysis functions. According to the software manual (ImageJ User Guide IJ 1.46r), the obtained "Feret" parameter represents the maximum spacing between all parallel lines in the two-dimensional projection of the particle, thus characterizing the particle size; the obtained "Area" parameter represents the pixel area of the particle. Because particles smaller than 50 nm are prone to significant errors during statistical analysis and are difficult to accurately identify, and because the particle size of conductive agents is generally smaller than 50 nm, which can also introduce large errors into the statistical results, particles smaller than 50 nm are not counted in the particle size statistics of this application, and the particle statistics corresponding to Area, Round, or Solidity values displaying as "NaN" are deleted. The sum of the "Area" parameters of particles with a diameter greater than or equal to 1 μm and the sum of the "Area" parameters of all particles are calculated and used as the area of particles with a diameter greater than or equal to 1 μm and the total area of the counted particles, respectively. The sum of the areas of particles with a diameter greater than or equal to 1 μm divided by the total area of the counted particles is used as the percentage of the area of particles with a diameter greater than or equal to 1 μm in the cross-section of the positive electrode film along the thickness direction of the electrode sheet.
[0121] In some embodiments, the area percentage of particles with a diameter greater than or equal to 1 μm in the cross-section of the positive electrode film along the electrode thickness direction can be selected as 12%, 12.02%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 3... 4%, 34.78%, 34.95%, 35%, 36%, 36.29%, 36.37%, 36.64%, 36.88%, 37%, 38%, 38.09%, 38.44%, 39%, 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49%, 49.96%, 50%, or any range of two.
[0122] In some embodiments, the area ratio of particles with a diameter greater than 50 nm and less than or equal to 200 nm in the cross-section of the positive electrode film along the electrode thickness direction is 3.0%-15.0%.
[0123] In the cross-section of the positive electrode film along the thickness direction of the electrode sheet, the area ratio of particles with a diameter greater than 50 nm and less than or equal to 200 nm can be obtained by referring to the test method for the area ratio of particles with a diameter greater than or equal to 1 μm described above.
[0124] In some embodiments, the area percentage of particles with a diameter greater than 50 nm and less than or equal to 200 nm in the cross-section of the positive electrode film along the electrode thickness direction can be selected as 3%, 4%, 5%, 5.33%, 5.91%, 6%, 6.35%, 6.42%, 6.49%, 6.52%, 6.54%, 6.55%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 14.81%, 15%, or any value range between the two.
[0125] Theoretical studies show that, under ideal conditions, spherical particles with a diameter of 314 nm can fill the gaps formed by the stacking of spherical particles with a diameter of 1 μm, thereby improving particle gradation and electrode compaction density. Particles with a diameter greater than 50 nm and less than or equal to 200 nm can tightly fill the gaps between particles greater than or equal to 1 μm, achieving dense packing. When the area ratio of particles with a diameter greater than 50 nm and less than or equal to 200 nm is within a suitable range, it is beneficial to improve the compaction density of the positive electrode through gradation, while avoiding an excessively high area ratio of small particles that would increase the internal resistance of the positive electrode film. This results in a battery with good capacity while further improving the battery's kinetic performance.
[0126] In some embodiments, the compaction density of the positive electrode sheet of the battery cell in a fully discharged state is 2.3 g / cm³. 3 -2.6g / cm 3 .
[0127] In this application, the fully discharged state refers to the state after the battery is placed in a 25°C oven environment, left to stand for 2 hours, and the battery temperature is maintained at 25°C, and then discharged at a constant current of 1 / 3C to 2.5V and then discharged at a constant current of 0.1C to 2.0V.
[0128] The compaction density of the positive electrode sheet can be tested using methods known in the art. As an example, the battery is placed in a 25°C oven environment and left to stand for 2 hours. After the battery temperature is maintained at 25°C, the battery is discharged at a constant current of 1 / 3C to 2.5V and then discharged at a constant current of 0.1C to 2.0V. The battery is then disassembled to obtain the positive electrode sheet. The residual electrolyte is treated with dimethyl carbonate solvent, the electrode sheet is dried, and it is cut into small circular pieces with an area of S. The mass of the circular pieces is obtained as W1, and the thickness of the positive electrode sheet is measured using a micrometer. Then, the positive electrode film layer of the weighed electrode sheet is wiped off, the mass of the current collector is weighed and recorded as W2, and the thickness of the current collector is measured using a micrometer. Then, the compaction density of the positive electrode sheet is PD=(W1-W2) / [(T1-T2)×S].
[0129] In some embodiments, the compaction density of the positive electrode sheet in the fully discharged state can be selected as 2.3 g / cm³. 3 2.31 g / cm 3 2.32 g / cm 3 2.33 g / cm 3 2.34 g / cm 3 2.35g / cm 3 2.36 g / cm 3 2.37 g / cm 3 2.38g / cm 3 2.39 g / cm 3 2.40 g / cm 3 2.41 g / cm 3 2.42 g / cm 3 2.43 g / cm 3 2.44 g / cm 3 2.45g / cm 3 2.46 g / cm 3 2.47 g / cm 3 2.48 g / cm 3 2.49 g / cm 3 2.50g / cm 3 2.51g / cm 3 2.52g / cm 3 2.53g / cm 3 2.54 g / cm 3 2.55g / cm 3 2.56 g / cm 3 2.57g / cm 3 2.58g / cm 3 2.59g / cm 3 2.60g / cm 3 Or the range of values between any two.
[0130] In some embodiments, the area of particles with a diameter greater than or equal to 1 μm and less than or equal to 5 μm in the cross-section of the positive electrode film along the electrode thickness direction accounts for 12%-50%.
[0131] When the area ratio of particles with a diameter greater than or equal to 1 μm and less than or equal to 5 μm in the cross-section of the positive electrode film along the thickness direction of the electrode sheet is within the above range, it is beneficial to further improve the phenomenon of film loosening and active material shedding caused by stress concentration when large particles are pressed into the electrode sheet, thereby improving the cycle performance of the battery while maintaining high capacity.
[0132] In some embodiments, the area of particles with a diameter greater than or equal to 1 μm and less than or equal to 5 μm in the cross-section of the positive electrode film along the electrode thickness direction accounts for 12%-40%.
[0133] When the area ratio of particles with a diameter greater than or equal to 1 μm and less than or equal to 5 μm in the cross-section of the positive electrode film along the thickness direction of the electrode sheet is within the above range, it is beneficial to further improve the phenomenon of film loosening and active material shedding caused by stress concentration when large particles are pressed into the electrode sheet, while maintaining high capacity, and further improve the cycle performance of the battery.
[0134] In some embodiments, the uniformity of particle distribution with a diameter greater than or equal to 1 μm in the cross-section of the positive electrode film layer along the electrode thickness direction is 0.2%-5%, and can be optionally 0.2%-2%.
[0135] The method for testing the uniformity of particle distribution with a diameter greater than or equal to 1 μm in a cross-section along the thickness direction of the positive electrode film can be performed using methods known in the art. As an example, the cross-section of the positive electrode film along the thickness direction is divided into three layers of equal thickness: a lower layer close to the positive current collector, an upper layer away from the positive current collector, and a middle layer between the upper and lower layers. Ten non-overlapping fields of view are selected in each of the upper, middle, and lower layers, and scanning electron microscope (SEM) images are taken at 10kx magnification. The 30 SEM images are imported into ImageJ software for analysis, and the area ratio of particles with a diameter greater than or equal to 1 μm in each of the 30 images is measured, resulting in 30 values. The range of these 30 values represents the uniformity of particle distribution with a diameter greater than or equal to 1 μm in a cross-section along the thickness direction of the positive electrode film, where the range is the difference between the maximum and minimum values among the 30 values. In the cross-section of the positive electrode film along the thickness direction of the electrode sheet, the smaller the uniformity of the distribution of particles with a diameter greater than or equal to 1 μm, the more uniform the distribution of large particles in the positive electrode film.
[0136] In some embodiments, the uniformity of particle distribution with a diameter greater than or equal to 1 μm in the cross-section of the positive electrode film along the electrode thickness direction can be selected as 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 1%, 2.1%, or 2.2%. 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 1%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 1%, 4.1%, 4.2%, 4.3%, 4.4%, 4.5%, 4.6%, 4.7%, 4.8%, 4.9%, 5%, or any range of two.
[0137] The uniformity of the distribution of particles with a diameter greater than or equal to 1 μm in the cross-section along the thickness direction of the positive electrode film is within a suitable range. The uniformly distributed large particles can effectively reduce the stress concentration in local areas of the film, so that the stress during the film compaction process can be uniformly dispersed throughout the entire area of the film, avoiding the local stress concentration caused by particle agglomeration, reducing the probability of film peeling, and improving the cycle performance of the battery.
[0138] In some embodiments, in the cross-section of the positive electrode film along the electrode thickness direction, the median L of the spheroidality in the cumulative distribution curve of the spheroidality area of particles with a diameter greater than or equal to 1 μm is... A50 It is 0.6-0.8.
[0139] The specific method for testing the sphericity of particles with a diameter greater than or equal to 1 μm in a cross-section of the positive electrode film along the electrode thickness direction is as follows: Particles with a diameter greater than or equal to 1 μm in a cross-section of the positive electrode film along the electrode thickness direction are identified using the method described above in this application. The morphology of the particles in the cross-section along the electrode thickness direction of the positive electrode film is analyzed using the "Shape Description" analysis function in ImageJ. According to the software manual (ImageJ User Guide IJ 1.46r), the "Round" parameter obtained from the analysis represents the ratio of the pixel area of the particle to the area of a circle with the fitted major axis as its diameter, which can be used to characterize the sphericity of the particle. The closer the particle is to a sphere, the closer the ratio of the pixel area to the area of the circle with the fitted major axis as its diameter is to 1. Therefore, the "Round" parameter of the particle obtained from the analysis is used to characterize the sphericity of the particle. Because particles smaller than 50 nm present significant errors during statistical analysis and are difficult to accurately identify, and because the particle size of conductive agents is generally smaller than 50 nm, which can also introduce substantial errors into the statistical results, particles smaller than 50 nm are not counted in the particle size statistics process of this application, and the statistical data for particles with a Round value of "NaN" are deleted. Following the above method, to ensure a statistically significant sample size, at least 10 non-overlapping scanning electron microscope (SEM) images were acquired for each electrode. The sphericity of at least 1000 particles was arranged in ascending order, and the cumulative sphericity distribution curve of the particles in the positive electrode film was obtained with sphericity as the horizontal axis and the cumulative area percentage as the vertical axis. A50 This is the L-value of sphericity that corresponds to the cumulative area ratio of the vertical axis in the cumulative distribution curve of granular sphericity L-values being 50%.
[0140] In some embodiments, in the cross-section of the positive electrode film along the electrode thickness direction, the median L of the spheroidality in the cumulative distribution curve of the spheroidality area of particles with a diameter greater than or equal to 1 μm is... A50The value can be selected from 0.60, 0.61, 0.62, 0.63, 0.64, 0.65, 0.66, 0.67, 0.68, 0.69, 0.70, 0.705, 0.71, 0.72, 0.73, 0.74, 0.75, 0.76, 0.77, 0.78, 0.79, 0.80, or any value range between the two.
[0141] The median sphericity of particles with a diameter of 1 μm or greater is within the above range. Larger particles have better sphericity, which reduces particle bridging caused by the irregular shape of large particles, reduces the void content in the electrode, and at the same time reduces the stress concentration aggravated by the irregularity of large particles. This improves the phenomenon of film loosening and active material shedding, and the battery cell has high capacity and good cycle performance.
[0142] Those skilled in the art can control the sphericity of particles using any known process. For example, the sphericity of particles can be adjusted through processes such as grinding, polishing, chemical etching, mechanical stirring, extrusion, coating, granulation, and adding surfactants, as well as by adjusting the parameters of each process.
[0143] In some embodiments, in the cross-section of the positive electrode film along the electrode thickness direction, the median L of the spheroidality in the cumulative distribution curve of the spheroidality area of particles with a diameter greater than or equal to 1 μm is... A50 It is 0.65-0.75.
[0144] The median sphericity of particles with a diameter of 1 μm or greater is within the above range, which helps to reduce stress concentration caused by the irregularity of large particles exacerbating electrode pressure, and improves the phenomenon of film loosening and active material shedding.
[0145] In some embodiments, in the cross-section of the positive electrode film along the electrode thickness direction, the median L of the spheroidality in the cumulative distribution curve of the spheroidality area of particles with a diameter greater than or equal to 1 μm is... A50 It is 0.67-0.75.
[0146] The median sphericity of particles with a diameter of 1 μm or greater is within the above range, which can further improve the stress concentration that occurs when large particles are pressed into the electrode, reduce the probability of film loosening and active material shedding, and improve the cycle life of the battery cell.
[0147] In some implementations, the area ratio of particles with a diameter greater than 50 nm and less than or equal to 200 nm is 5.0%-15.0%.
[0148] The area ratio of particles with a diameter greater than 50nm and less than or equal to 200nm is within the above range. The positive electrode film layer has an appropriate amount of small particles, which ensures sufficient particle filling degree, while avoiding the adverse effect of excessive small particle area ratio on the film layer resistance. The battery improves the dynamic performance of the battery while having good capacity.
[0149] In some implementations, the area ratio of particles with a diameter greater than 50 nm and less than or equal to 200 nm is 5.0%-10.0%.
[0150] When the area ratio of particles with a diameter greater than 50nm and less than or equal to 200nm is within the above range, the positive electrode film has a good particle size distribution, which further reduces the resistivity of the positive electrode film and further improves the dynamic performance of the battery on the basis of good capacity.
[0151] In some implementations, the thickness of the positive electrode film on one side is 70 μm-120 μm.
[0152] The thickness of the positive electrode film can be measured using any method known in the art. As an example, the thickness of the positive electrode film in a cross-section along the thickness direction of the positive electrode sheet is measured using a scanning electron microscope. Measurements are taken at three randomly selected locations, and the average value is taken as the thickness of the positive electrode film.
[0153] In some embodiments, the single-sided thickness of the positive electrode film can be selected as 70 μm, 72.34 μm, 71 μm, 72 μm, 73 μm, 74 μm, 75 μm, 76 μm, 77 μm, 78 μm, 79 μm, 80 μm, 81 μm, 82 μm, 83 μm, 83.91 μm, 84 μm, 85 μm, 86 μm, 87 μm, 88 μm, 89 μm, 90 μm, 91 μm, 91.88 μm, 92 μm, 93 μm, 94 μm, 95 μm, 96 μm, 97 μm, 98 μm, 98.93 μm, 99 μm. m, 100μm, 101μm, 102μm, 103μm, 104μm, 105μm, 105.44μm, 105.64μm, 105.65μm, 105.89μm, 106μm, 106.21μm, 106.34μm, 107 μm, 108μm, 109μm, 110μm, 111μm, 112μm, 113μm, 114μm, 115μm, 116μm, 116.09μm, 117μm, 118μm, 119μm, 120μm or any numerical range between the two.
[0154] The specific capacity of lithium-containing transition metal phosphate particles is relatively low. Studies have shown that when the single-sided thickness of the positive electrode film is less than 70 μm, the battery capacity is difficult to meet market demand. A single-sided thickness of the positive electrode film within the aforementioned range is beneficial for improving the capacity of individual battery cells.
[0155] In some implementations, the thickness of the positive electrode film on one side is 90 μm-120 μm.
[0156] A single-sided thickness of the positive electrode film within the above-mentioned range is beneficial for further improving the capacity of the battery cell.
[0157] In some implementations, the thickness of the positive electrode film on one side is 100 μm-120 μm.
[0158] Increasing the thickness of the positive electrode film on one side is beneficial to improving the battery capacity. The applicant found that when the thickness of the positive electrode film on one side is greater than or equal to 100 μm, the positive electrode film is more prone to loosening and shedding of active material. The embodiments of this application reduce the area ratio of large particles and reduce the compaction density of the positive electrode film, which together improves the stress concentration phenomenon of large particles in the stacked cell during electrode compaction. At the same time, an appropriate amount of small particles are added so that the electrode can still have a good compaction density while giving up a certain amount of large particles, and the battery has a good capacity and cycle performance.
[0159] In some embodiments, the positive electrode film layer further includes a conductive agent, and the total area of the agglomerated region of the conductive agent accounts for 0.2%-6%, optionally 1.5%-5%, based on the total area of the cross section of the positive electrode film layer along the thickness direction of the electrode sheet.
[0160] Based on the total area of the cross-section along the thickness direction of the positive electrode film, the total area ratio of the agglomeration region of the conductive agent within the above range indicates that the conductive agent in the positive electrode film is uniformly dispersed and easily forms a uniform conductive network, which is beneficial to reducing local polarization and even lithium plating problems generated during battery cycling.
[0161] Meanwhile, the appropriate amount of small particles in this application can serve as a basic conductive framework to fill the gaps between large particles, while the dispersed conductive agent agglomerates serve as long-range conductive nodes, forming a hierarchical conductive structure. Since large particles in lithium transition metal phosphate particles are prone to rebound, the agglomeration area of the conductive agent within the above-mentioned range can also suppress the rebound of large particles by means of the uniform distribution of the conductive agent, forming mechanical constraints on the particles and even the film layer, improving the cohesion of the film layer, reducing the phenomenon of film layer powder shedding and active material shedding, and improving the cycle life of the battery.
[0162] The area ratio of conductive agent agglomeration regions can be tested using the following method, based on the total area of the cross-section of the positive electrode film along the electrode thickness direction. Using a method similar to that described above, the cross-section of the positive electrode film along the electrode thickness direction is observed using a scanning electron microscope (SEM), and the area of the conductive agent agglomeration region in the SEM image is measured at 3kx magnification. Since conductive agents are generally carbon-based materials, such as conductive carbon black and carbon nanotubes, the conductive agent agglomeration region often appears as a black agglomeration compared to other areas in the positive electrode film. At high magnification, the aggregated conductive agent can be seen. The conductive agent agglomeration region refers to the area in the SEM image where the conductive agent is clearly aggregated and appears black. Using image analysis software, such as ImageJ, the white-marked areas are selected to identify regions with a Feret value greater than or equal to 2 μm. The sum of the areas of these regions is the total area of the conductive agent agglomeration region in the SEM image. The area ratio of the conductive agent agglomeration region is characterized by dividing the total area of the conductive agent agglomeration region measured in the SEM image at 3kx magnification by the area of the SEM image. Three non-overlapping scanning electron microscope images are randomly selected, and the average value is calculated as "the total area ratio of the agglomeration region of the conductive agent based on the total area of the cross section along the thickness direction of the positive electrode film".
[0163] In some embodiments, the conductive agent includes carbon nanotubes, which include one or more of single-walled carbon nanotubes, few-walled carbon nanotubes, and multi-walled carbon nanotubes. Optionally, the conductive agent also includes conductive carbon black.
[0164] Carbon nanotubes have a high aspect ratio, which is beneficial for bridging particles of different sizes in the thickness direction through their unique fiber structure. This forms a long-range conductive path while increasing the binding force between particles, reducing local polarization and even lithium plating problems during battery cycling, and improving the cycle life of the battery. Furthermore, through the binding effect, it can reduce the rebound phenomenon of large particles in the positive electrode film and reduce the shedding of active materials in the film.
[0165] Conductive carbon black, with its nanoscale size, tightly coats the surface of the positive electrode active particles, forming high-density point-like conductive contacts. When used in conjunction with carbon nanotubes, it balances both long-range and short-range conductivity, further improving the conductive network within the positive electrode film. The high specific surface area of conductive carbon black significantly enhances electrolyte adsorption capacity, effectively mitigating electrolyte consumption during cycling; the mechanical toughness of carbon nanotubes buffers electrode expansion stress; the synergistic effect of both reduces electrolyte extrusion caused by the high increase in expansion force during long cycles, thus improving the battery's cycle life.
[0166] In some embodiments, the agglomeration regions of the conductive agent include carbon nanotubes and conductive carbon black.
[0167] Researchers have found that carbon nanotubes are prone to agglomeration due to their high surface energy, which leads to uneven dispersion in the positive electrode film layer and fails to form an effective carbon nanotube network structure. The surface energy of conductive carbon black is relatively close to that of carbon nanotubes, so it can adsorb on the surface of carbon nanotubes to form a physical barrier, increase the resistance to agglomeration of carbon nanotubes, reduce direct contact between carbon nanotubes, thereby inhibiting the agglomeration phenomenon and improving the distribution uniformity of carbon nanotubes in the positive electrode film layer. On the one hand, this helps to improve the conductivity of the positive electrode film layer and enhance the dynamic performance of the battery; on the other hand, it helps to exert the binding effect of carbon nanotubes on the positive electrode film layer, reduce the risk of the positive electrode film layer falling off, and further improve the dynamic performance and cycle life of the battery. In addition, the agglomeration of carbon nanotubes in the agglomerated region of the conductive agent will also cause blockage of local ion transport paths in the agglomerated region of the conductive agent. The matching of conductive carbon black can improve the lithium ion transport capacity in this region, reduce local polarization, and further improve the cycle stability of the battery.
[0168] In some embodiments, based on the mass of the positive electrode film layer, the mass content C1 of carbon nanotubes satisfies: 0<C1≤2.5%, and the mass content C2 of conductive carbon black satisfies: 0<C2≤2.5%.
[0169] In some embodiments, based on the mass of the positive electrode film layer, the mass content C1 of carbon nanotubes can be selected as 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5% or any numerical range between any two of them.
[0170] In some embodiments, based on the mass of the positive electrode film layer, the mass content C2 of conductive carbon black can be selected as 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5% or any numerical range between any two of them.
[0171] When the mass contents of carbon nanotubes and conductive carbon black are within the above ranges, the agglomeration of carbon nanotubes can be effectively alleviated and a good conductive network structure can be formed, thereby effectively reducing the stress concentration of the positive electrode film layer, improving the liquid retention rate of the positive electrode film layer during long cycles, further reducing the risk of electrode plate film layer falling off and the degree of polarization, enhancing the dynamic performance of the battery and improving the cycle life of the battery.
[0172] In some embodiments, the positive electrode film layer further includes a dispersant, which includes hydrogenated nitrile butadiene rubber (HNBR).
[0173] The polar groups (such as cyano, -CN) in hydrogenated nitrile butadiene rubber (HNBR) molecules can interact with hydroxyl groups (-OH) or metal oxide sites on the surface of lithium transition metal phosphate particles (such as hydrogen bonding, dipole interaction), enhancing the compatibility between particles and solvents, reducing the interfacial tension between particles and solvents, and improving the interfacial tension of large particles more significantly. This makes it easier for large and small particles in the film to be evenly dispersed, reducing particle aggregation caused by hydrophobicity, improving the dispersibility of large particles in the positive electrode film, and reducing stress concentration generated during the film die-cutting process.
[0174] Meanwhile, during the drying and film formation of the slurry, the elastic network structure of HNBR can buffer the shrinkage stress caused by solvent evaporation, reduce the re-aggregation of conductive agents due to capillary forces during this process, reduce the area ratio of conductive agent agglomeration regions, and the uniform distribution of conductive agents helps to suppress the rebound of large particles, forming mechanical constraints on particles and even film layers, improving the cohesive force of film layers, reducing film layer powder shedding and active material shedding, and improving the cycle life of the battery.
[0175] In some implementations, the mass content of the dispersant is 0.5%-2% based on the mass of the positive electrode film.
[0176] In some embodiments, based on the mass of the positive electrode film, the mass content of the dispersant can be selected as 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2%, or any value range between the two.
[0177] When the mass content of the dispersant is within the above range, it can achieve uniform dispersion of particles in the positive electrode film while maintaining a high loading capacity, resulting in good capacity and cycle performance of the battery.
[0178] In some embodiments, the positive electrode film layer has a base coating layer in the bottom region near the positive electrode current collector. The base coating layer includes a conductive agent and a binder. The conductive agent includes carbon nanotubes and conductive carbon black, and the binder includes vinylidene fluoride polymer.
[0179] In some embodiments, the thickness of the base coating is 0.5 μm to 5 μm.
[0180] In some embodiments, the thickness of the base coating can be selected as 0.5 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm or any value range between the two.
[0181] The undercoating layer provided in this application helps improve the adhesion between the positive electrode film and the positive electrode current collector and alleviates stress concentration at large particles, thereby reducing the probability of positive electrode film detachment and improving the cycle stability of the battery. Simultaneously, compared to direct contact between the positive electrode current collector and the positive electrode film, the increased contact area between the undercoating layer and the positive electrode film helps increase the area for electron transport between the current collector and the positive electrode film, thereby reducing the internal resistance of the electrode and improving the battery's dynamic performance.
[0182] In some embodiments, the median C of the graphitization degree C in the cumulative distribution curve of the positive electrode film obtained in laser microscopy confocal Raman spectroscopy instrument scanning mode is... 50 Greater than or equal to 0.95 and less than or equal to 1.20; wherein, the degree of graphitization C is I. G / I D I G This indicates that the Raman spectrum is at 1580±100 cm⁻¹ -1 The intensity of peak G at I D This indicates that the Raman spectrum is at 1350±100 cm⁻¹ -1 The intensity of peak D at that location.
[0183] In this application, the graphitization degree C value of the positive electrode film can be obtained by surface scanning mode of a laser confocal Raman spectrometer. As an example, specifically, a laser confocal Raman spectrometer (high-precision Renishaw laser confocal Raman spectrometer) is used, with an excitation wavelength of 532 nm. An appropriate amount of the positive electrode film is taken and surface scanned on its surface or along the cross-section of the electrode thickness. The scanning area is 45 μm × 45 μm, divided into 10 × 10 grids, with grid vertices as test points, a step size of 5 μm, and a total of 100 scan points. Thus, the C values at different sites and the cumulative distribution curve of the C values in the surface scan area are obtained.
[0184] The positive electrode film in this application can be either a freshly prepared positive electrode film or a positive electrode film obtained from disassembly of a battery. The surface of a positive electrode film obtained from disassembly of a battery inevitably contains residual electrolyte salt particles. To improve testing accuracy, it is preferable to perform a surface scan on a cross-section of the positive electrode film along the electrode thickness direction to characterize the degree of graphitization of the positive electrode film.
[0185] The graphitization degree C of the positive electrode film was obtained by the ratio of the peak intensities of the G-band and D-band in the Raman spectrum. The position of the G-band peak was 1580±100 cm⁻¹. -1 Its characterization of carbon sp 2 Hybrid structure; D peak position is 1350±100 cm⁻¹ - 1 It characterizes the disordered structure of carbon, where disorder refers to the irregular arrangement of carbon atoms in the structure.
[0186] The cumulative distribution curve of graphitization degree C value refers to the curve obtained by arranging at least 100 C values in ascending order, with graphitization degree as the horizontal axis and the cumulative percentage as the vertical axis. 50 This represents the C value corresponding to a cumulative percentage of 50% on the vertical axis of the cumulative distribution curve of graphitization degree C. The median C value of graphitization degree. 50 Compared to point values, it can reflect the overall graphitization degree of particles in the positive electrode film, i.e., the degree of slippage; compared to the mean value, it can reduce the influence of extreme values during the test and improve the confidence of the test results.
[0187] Those skilled in the art can control the degree of graphitization of active material particles using any known process. For example, adjusting the carbon source, sintering temperature, sintering time, sintering pressure, and sintering atmosphere can all achieve adjustments to the degree of graphitization of active material particles.
[0188] In some embodiments, the median C of the graphitization degree C in the cumulative distribution curve of the positive electrode film obtained in laser microscopy confocal Raman spectroscopy instrument scanning mode is... 50 The value can be selected from 0.95, 0.96, 0.97, 0.98, 0.99, 1.0, 1.01, 1.02, 1.03, 1.04, 1.05, 1.06, 1.07, 1.08, 1.09, 1.1, 1.11, 1.12, 1.13, 1.14, 1.15, 1.16, 1.17, 1.18, 1.19, 1.20, or any value range between the two.
[0189] In the cumulative distribution curve of graphitization degree C obtained by laser microscopy confocal Raman spectroscopy in instrument scanning mode, the median C of graphitization degree is... 50 Within the aforementioned range, the compaction density of the electrode can be further improved by relying on particle slippage, without overly relying on the ratio of large to small particles in the positive electrode film. This ensures that the area ratio of large and small particles is within a suitable range, which helps reduce the probability of positive electrode film shedding and avoids excessive resistance of the positive electrode film. This helps improve the cycle performance and dynamic performance of the battery while maintaining its capacity.
[0190] In some embodiments, the lithium transition metal phosphate particles in the positive electrode film layer comprise components represented by the following general formula:
[0191] Li m Fe x P y O j Q q Formula I,
[0192] Wherein, Q includes one or more of Al, Na, K, Mg, Cu, Mn, Cr, Zn, Pb, Ca, Co, Ni, Sr, Nb, V, Ti, B, S, Si, N, F, Cl, and Br, with 0.8≤m≤1.15, 0.9≤x≤1, 0.95≤y≤1, 3.5≤j≤4, and 0≤q≤0.1.
[0193] In some implementations, m can be selected as 0.8, 0.85, 0.9, 0.95, 0.98, 1.00, 1.03, 1.05, 1.08, 1.10, 1.13, 1.15, or any value range between two of these; x can be selected as 0.9, 0.91, 0.92, 0.93, 0.94, 0.95, 0.96, 0.97, 0.98, 0.99, 1.0, or any value range between two of these. y can be 0.95, 0.96, 0.97, 0.98, 0.99, 1.00 or any value between two of these; j can be 3.5, 3.6, 3.7, 3.8, 3.9, 4 or any value between two of these; q can be 0, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1 or any value between two of these.
[0194] In some embodiments, the lithium-containing transition metal phosphate particles include titanium, and the mass content of titanium is 500ppm-8000ppm, optionally 1000ppm-3000ppm, based on the total mass of the lithium-containing transition metal phosphate particles in the positive electrode film.
[0195] In some embodiments, the titanium element is uniformly distributed in lithium-containing transition metal phosphate particles.
[0196] The types and contents of elements in lithium transition metal phosphate particles in the positive electrode film can be tested using any method known in the art. As an example, inductively coupled plasma atomic emission spectrometry (ICP-AES) was used to test the titanium content, referring to Appendix C of GB / T 33822-2017.
[0197] When titanium is doped into lithium-containing transition metal phosphate particles, the Ti-OP bonds formed have a strong bonding effect. By anchoring phosphate groups, the contraction / expansion of the lattice during lithium ion insertion / extraction is reduced, thereby suppressing the structural stress caused by phase transition and improving the cycle life of the battery. In addition, the Ti-OP bonds can provide a more stable channel for lithium ion diffusion, reduce the migration energy barrier, and improve the kinetic performance of the battery.
[0198] Within the above-mentioned range, the mass content of titanium is beneficial to improving the lithium-ion transport rate of the positive electrode active material, reducing the risk of lithium plating, and improving the kinetic performance of the battery.
[0199] In some embodiments, the mass content of titanium can be selected from 500ppm, 1000ppm, 1500ppm, 2000ppm, 2500ppm, 3000ppm, 3500ppm, 4000ppm, 4500ppm, 5000ppm, 5500ppm, 6000ppm, 6500ppm, 7000ppm, 7500ppm, 8000ppm, or any value range between the two, based on the total mass of lithium transition metal phosphate particles in the positive electrode film.
[0200] In some embodiments, the lithium-containing transition metal phosphate particles include vanadium, and the vanadium content is 500ppm-5000ppm, optionally 500ppm-3000ppm, based on the total mass of the lithium-containing transition metal phosphate particles in the positive electrode film.
[0201] In some embodiments, the vanadium element is uniformly distributed in lithium-containing transition metal phosphate particles.
[0202] When vanadium is doped into lithium-containing transition metal phosphate particles, it exhibits multiple valence states. For example, vanadium in the +5 valence (V+5) has a multivalent state. 5+ Phosphorus doping, due to its larger radius, introduces lattice distortion, expands lithium-ion diffusion channels, and improves the ionic conductivity of the positive electrode active material; when +3 valent vanadium (V... 3+ Doping with transition metal sites allows for charge compensation through lithium vacancies or interstitial oxygen, forming defect energy levels and improving the electronic conductivity of the positive electrode active material.
[0203] Vanadium content within the above range is beneficial for improving the lithium-ion transport rate of the cathode active material, enhancing its electronic conductivity, and further improving the battery's kinetic performance through synergistic effects with titanium doping.
[0204] In some embodiments, based on the total mass of lithium transition metal phosphate particles in the positive electrode film, the mass content of vanadium can be selected as 500ppm, 1000ppm, 1500ppm, 2000ppm, 2500ppm, 3000ppm, 3500ppm, 4000ppm, 4500ppm, 5000ppm or any range between the two.
[0205] In some embodiments, the lithium-containing transition metal phosphate particles in the positive electrode film include one or more of lithium iron phosphate, lithium manganese phosphate, lithium vanadium fluoride phosphate, lithium manganese iron phosphate, and their modified materials.
[0206] In some embodiments, the lithium-containing transition metal phosphate particles in the positive electrode film include one or more of lithium iron phosphate and its doped and modified materials, and coating and modified materials.
[0207] In some implementations, the porosity of the positive electrode film is 14%-28%.
[0208] The porosity of the positive electrode film can be tested as follows: Import the cross-sectional SEM image of the positive electrode film along the thickness direction obtained as described above into ImageJ software. Select the line tool and use a line to mark the length of the scale bar in the image. Click "Analyze Set Scale" and set the scale parameters in the software according to the scale bar length in the image. Select the rectangle tool and select the part of the image outside the scale bar area. Use "Image Duplicate" to copy the selected area and use "Image Type 8bit" to adjust the image format. Select "Analyze Set Measurements" and choose the following 5 options: "Area", "Mean gray value", "Area Fraction", "Limit to threshold", and "Feret's diameter". Select 3 for "Decimal places". Then select "Image" - "Adjust" - "Threshold" in sequence and set 0 and 100 in the "Threshold" box. You can then use the Analyze-Measure function to export the porosity data from the cross-sectional SEM image. Export using "Image" - "Overlay" - "Flatten" to obtain a pore image; click "Apply" in "Threshold", then click "Analyze" - "Analyze Particles", check the four columns on the left to obtain pore statistics.
[0209] It is understood that in the embodiments of this application, "pores" in the cross-section of the positive electrode film are identified by image color difference and threshold. These "pores" are not pore data obtained from the degassing test, but are mainly used to characterize the cross-sectional area between particles in the cross-section of the positive electrode film. This method is superior to the degassing method because the porosity obtained by the degassing method is related to the pores between particles and the pores in the carbon material on the surface of the lithium iron phosphate particles, thus failing to objectively reflect the pores between particles.
[0210] A porosity within the above-mentioned range in the positive electrode film indicates a better particle size distribution in the positive electrode film, which is beneficial for improving the electrolyte retention characteristics, improving the ion diffusion of the positive electrode film with a certain area ratio of large particles, and improving the kinetic performance of the battery.
[0211] In some embodiments, the porosity of the positive electrode film can be selected as 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, or any value range between the two.
[0212] In some implementations, the resistivity of the positive electrode film is 10 Ω·cm to 35 Ω·cm.
[0213] The resistivity of the positive electrode film can be tested by the following method: a resistance tester (Suzhou Lidian) is used to test under a standard pressure of 25MPa. During the test, 8 test points are randomly selected on the film of the positive electrode sheet. The pressure is maintained at each test point for 15s to obtain the resistivity at that test point. The average value of the 8 resistivities is taken as the resistivity of the positive electrode film.
[0214] In some embodiments, the resistivity of the positive electrode film can be selected from 10 Ω·cm, 11 Ω·cm, 12 Ω·cm, 13 Ω·cm, 14 Ω·cm, 15 Ω·cm, 16 Ω·cm, 17 Ω·cm, 18 Ω·cm, 19 Ω·cm, 20 Ω·cm, 21 Ω·cm, 22 Ω·cm, 23 Ω·cm, 24 Ω·cm, 25 Ω·cm, 26 Ω·cm, 27 Ω·cm, 28 Ω·cm, 29 Ω·cm, 29.72 Ω·cm, 29.88 Ω·cm, 30 Ω·cm, 30.55 Ω·cm, 30.73 Ω·cm, 31 Ω·cm, 31.5 Ω·cm, 32 Ω·cm, 32.2 Ω·cm, 33 Ω·cm, 33.67 Ω·cm, 34 Ω·cm, 34.98 Ω·cm, 35 Ω·cm, or any value between the two.
[0215] When the resistivity of the positive electrode film is within a suitable range, it is beneficial to reduce electron transport impedance, reduce charge and discharge polarization, and improve the dynamic performance of the battery.
[0216] In some embodiments, as shown in FIG1, the battery cell further includes a separator 20 disposed between the positive electrode and the negative electrode. The separator 20 includes a base film 201, ceramic layers 202 disposed on both sides of the base film 201, and an adhesive layer 203 disposed on at least one side of the ceramic layer 202 away from the base film 201. The adhesive layer 203 is a continuous layer with a porous structure and includes a vinylidene fluoride polymer.
[0217] In some embodiments, the vinylidene fluoride polymer includes vinylidene fluoride homopolymer (PVDF) and copolymers of vinylidene fluoride with other monomers, such as copolymers of vinylidene fluoride and hexafluoropropylene.
[0218] As shown in Figure 2, in the prior art, the adhesive layer of the diaphragm often uses aqueous PVDF, which often presents an island-like structure in the diaphragm. This is beneficial for providing gaps for cell expansion and is also convenient for manufacturing. However, such a diaphragm adhesive layer has a low bonding area and weak adhesion.
[0219] Figure 3 shows a schematic diagram of the surface morphology of the adhesive layer 203 of the separator in this embodiment of the application. The adhesive layer of the separator in this embodiment of the application has a certain porous structure in its continuous structure. Through the porous structure, the ceramic layer disposed between the base film and the adhesive layer can be observed. It is understood that when a porous continuous layer is used as the adhesive layer, it may become blocky due to contact with the positive or negative electrode or being squeezed during electrode manufacturing or cycling. The continuous layer referred to in this application does not require the adhesive layer to be continuous throughout the entire battery; rather, it refers to a continuous layer with a uniform porous structure at the microscopic level, such as when observed under a microscope, rather than an island-like structure. In order to reflect the true morphology of the separator, during the sampling process, it is preferable to sample in areas of the battery where the separator adhesive layer has less adhesion to the positive or negative electrode. For example, sampling can be performed at the position of the separator where the projection exceeds the positive and negative electrode; or sampling can be performed on the separator near the surface of the electrode assembly. The separator sampled in this way can better reflect the true state of the separator.
[0220] The separator provided in this application uses a continuous porous layer as the adhesive layer, which has a larger bonding area compared to the island-shaped adhesive layer in the prior art. This results in a stronger and more uniform bond between the separator and the positive electrode film. Simultaneously, the porous structure in the adhesive layer allows for both lithium-ion transport efficiency and improved battery dynamics. Furthermore, compared to wound cells, stacked cells experience less clamping force between the electrodes during cell fabrication. Lithium-containing transition metal phosphate particles with a diameter greater than or equal to 1 μm can reduce the tightness of internal components during rebound, increasing cell impedance and the probability of film shedding or even detachment. The separator provided in this application, using a continuous porous layer as the adhesive layer, is particularly suitable for stacked cells, improving the rebound phenomenon during long-cycle operation and enhancing battery capacity retention. Additionally, during the dragging of outer electrodes and welding of tabs, stacked cells are prone to relative displacement between the electrodes and the separator, making the film susceptible to powder shedding and even the positive and negative electrodes overlapping, posing a risk of internal short circuits.
[0221] This application embodiment uses a continuous layer with a porous structure as an adhesive layer to improve the adhesion between the separator and the electrode while maintaining the air permeability and porosity of the separator, thereby improving the stability of the electrode and further reducing the risk of powder shedding or even internal short circuit due to relative displacement between the electrode and the separator, thus improving the cycle stability of the battery.
[0222] In some embodiments, as shown in FIG4, the battery cell 5 includes a housing 50, the stacked cells are housed in the housing 50, the housing 50 has a length direction (X direction) dimension L0, a width direction (Y direction) dimension W0, and a thickness direction (Z direction) dimension H0, where 450mm≤L0≤1300mm, 100mm≤W0≤150mm, and 14mm≤H0≤22mm.
[0223] The casing size of the battery cell in this embodiment is within the above-mentioned range, which is beneficial for the battery to achieve a better capacity.
[0224] In some implementations, L0 can be selected as 450mm, 460mm, 470mm, 480mm, 490mm, 500mm, 510mm, 520mm, 530mm, 540mm, 550mm, 560mm, 570mm, 580mm, 590mm, 600mm, 610mm, 620mm, 630mm, 640mm, 650mm, 660mm, 670mm, 680mm, 690mm, 700mm, 710mm, 720mm, 750mm, 800mm, 850mm, 900mm, 950mm, 1000mm, 1050mm, 1100mm, 1150mm, 1200mm, 1250mm, 1300mm, or any value range between the two.
[0225] In some implementations, W0 can be selected as 100mm, 110mm, 120mm, 130mm, 140mm, 150mm or any value range between the two.
[0226] In some implementations, H0 can be selected as 14mm, 15mm, 16mm, 17mm, 18mm, 19mm, 20mm, 21mm, 22mm or any value range between the two.
[0227] In some embodiments, the length dimension L0 of the housing satisfies: 450mm≤L0≤650mm.
[0228] When the length dimension L0 of the casing satisfies 450mm≤L0≤650mm, the battery cell has a shorter length, which is beneficial to shorten the electron transport path, reduce the internal resistance of the battery, reduce the wetting distance of the electrolyte in the electrode pores, improve the wetting uniformity, and improve the dynamic performance of the battery. Especially under fast charging conditions, it can reduce the phenomenon of uneven temperature rise and uneven current density in the length direction of the electrode.
[0229] In some implementations, the length dimension L0 of the housing satisfies: 900mm≤L0≤1300mm.
[0230] When the length dimension L0 of the casing satisfies 900mm≤L0≤1300mm, the significantly increased single-cell size can effectively simplify the traditional module structure, enabling the single cell to be directly integrated into the battery pack. The battery is fixed by structural components set at the end of the large surface, which significantly improves the space utilization rate, thereby increasing the overall capacity of the battery system in the same volume, while reducing the number of structural components, increasing the battery energy density, and further improving the battery capacity.
[0231] In some embodiments, as shown in FIG4, the material of the housing 50 is a soft-pack material, which includes an aluminum-plastic composite film. Optionally, it includes one or more of polypropylene (PP), polybutylene terephthalate (PBT), polybutylene succinate (PBS), nylon, polyethylene terephthalate (PET), and polyethylene (PE) forming a composite film with aluminum.
[0232] Pouch cells possess high elongation, resulting in thin, flexible casings that improve space utilization and thus energy density. However, pouch cells, such as aluminum-plastic composite films, have poor thermal conductivity, leading to lower heat dissipation efficiency. Therefore, excessively high particle area in the positive electrode film increases resistivity, causing excessive heat generation during cycling and exacerbating the heat dissipation problem. This application addresses this issue by using pouch cells as the casing and controlling the particle area ratio in the positive electrode film within a suitable range, resulting in high capacity and good cycle performance.
[0233] In some embodiments, continuing to refer to FIG4, the housing 50 includes a first sealing area 51, which is disposed at at least one end of the laminated cell extending in the width direction (Y direction); the first sealing area 51 includes a folded edge structure extending in the length direction (X direction), and an encapsulating adhesive is disposed on the folded edge structure, which is continuously disposed in the length direction (X direction) and fixes the folded edge structure.
[0234] A folded edge structure refers to a reinforced structure formed by folding the encapsulation area in half. There is no limit to the number of folds. As an example, it can be a single folded edge structure with one fold or a double folded edge structure with folds on both sides.
[0235] During electrode cycling, the SEI film thickens, leading to significant rebound and gas generation during long cycles. The sealing area of the pouch cell is used to seal the electrode assembly, but the sealing area has limited strength and is easily broken open by large rebounds and high gas generation within the film layer.
[0236] This application embodiment further enhances the sealing strength of the first sealing area by including a folded edge structure extending along the length direction. The continuous arrangement of the encapsulating adhesive along the length direction and the fixing of the folded edge structure, compared to a discontinuous arrangement of the encapsulating adhesive along the length direction, further improves the sealing strength, achieving continuous reinforcement of the sealing area along its length and reducing the probability of the electrode breaking open the sealing area in the packaging during cycling.
[0237] In some embodiments, the housing 50 includes at least one second sealing area 52, which is disposed along the length of the housing at at least one end of the laminated cell, and the second sealing area 52 is disposed on the tab side of the laminated cell.
[0238] It is understandable that the positive and negative electrodes can be located on the same side of the laminated cell, as shown in Figure 4; or they can be located on opposite sides of the laminated cell.
[0239] In some embodiments, the battery cell 5 further includes a lead 53 connected to the tab of the battery cell. For example, the lead 53 can be soldered to the tab. The lead 53 is a conductive element, and at least a portion of the lead 53 is located outside the housing 50. The lead 53 serves as the electrode lead-out end of the battery cell 5, facilitating electrical connection between the battery cell 5 and other battery cells 5 or other components. For example, the lead 53 can be in the form of a sheet.
[0240] Correspondingly, lead-out element 53 also includes a positive lead-out element and a negative lead-out element, with the positive lead-out element connected to the positive electrode tab and the negative lead-out element connected to the negative electrode tab.
[0241] The second sealing area is located on the tab side. The tab needs to be connected to the lead-out component. The connection strength between the lead-out component and the shell material is relatively weak, which makes it easy for gas to escape from the second sealing area. This is conducive to directional pressure relief of the battery, reducing the impact on adjacent cells during thermal runaway, and improving the overall service life of the battery.
[0242] In some embodiments, the outer periphery of the laminated cell is provided with a plurality of rubber rings that surround in the width direction, and the rubber rings that surround in the width direction are spaced apart in the length direction.
[0243] The rubber rings that wrap around the width of the cell and are spaced apart along the length help to fix the position between the electrodes in the cell, reducing the probability of cell displacement during battery shaking. This is especially suitable for batteries with a large length, as it can effectively reduce the mutual displacement between the electrodes in the length direction, thus reducing lithium plating. This helps to maintain the stability of the internal spatial structure of the battery, thereby not affecting the normal operation of the battery.
[0244] In some embodiments, at 25°C, the capacity of the battery cell is 100Ah-300Ah, optionally 110Ah-190Ah, and further optionally 125Ah-180Ah.
[0245] In this application, the capacity of a single battery cell has a meaning known in the art and can be tested using methods known in the art. As an example, at 25°C, the battery cell is charged to 3.65V at a charging rate of 0.5C (the nominal capacity of the single cell), then charged at a constant voltage of 3.65V to 0.05C, left to stand for 10 minutes, and then discharged to 2.5V at a discharging rate of 1C, left to stand for 10 minutes. The capacity C during the discharge process is calculated using the formula C = I*t, with the unit being Ah.
[0246] In some embodiments, at 25°C, the capacity of the battery cell can be selected as 100Ah, 125Ah, 130Ah, 135Ah, 140Ah, 145Ah, 150Ah, 155Ah, 160Ah, 165Ah, 170Ah, 175Ah, 180Ah, 185Ah, 190Ah, 300Ah, or any value range between the two.
[0247] The battery cell in this application embodiment uses a suitable housing size to accommodate the stacked cells, and controls the proportion of large particles in the film layer of the positive electrode in the stacked cells to be reasonable, so that the battery cell has a high capacity.
[0248] In some embodiments, the positive current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer substrate and a metal layer formed on at least one surface of the polymer substrate. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0249] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer substrate and a metal layer formed on at least one surface of the polymer substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0250] In some embodiments, the negative electrode film layer includes a negative electrode active material. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, and hard carbon. However, this application is not limited to these materials, and other conventional materials that can be used as battery negative electrode active materials may also be used. These negative electrode active materials may be used alone or in combination of two or more.
[0251] In some embodiments, the negative electrode film layer may optionally include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).
[0252] In some embodiments, the negative electrode film may optionally include other additives, such as thickeners (e.g., sodium carboxymethyl cellulose (CMC-Na)).
[0253] In some embodiments, the negative electrode sheet can be prepared by dispersing the components used to prepare the negative electrode sheet, such as the negative electrode active material, conductive agent, binder and any other components, in a solvent (e.g., deionized water) to form a negative electrode slurry; coating the negative electrode slurry onto the negative electrode current collector, and then obtaining the negative electrode sheet after drying, cold pressing and other processes.
[0254] A second aspect of this application provides a battery device, including the battery cell provided in the first aspect of this application.
[0255] The battery device disclosed in this application can be used in electrical devices that use the battery device as a power source or in various energy storage systems that use the battery device as an energy storage element. Besides vehicles, the battery device can also be used in, but is not limited to, mobile phones, tablets, laptops, electric toys, power tools, electric vehicles, electric cars, ships, spacecraft, etc. Electric toys can include stationary or mobile electric toys, such as game consoles, electric car toys, electric ship toys, and electric airplane toys, etc. Spacecraft can include airplanes, rockets, space shuttles, and spacecraft, etc.
[0256] In addition, this application also provides an electrical device that uses a battery as a power source, the electrical device including at least one of the battery cell, battery module, or battery pack provided in this application. The battery cell, battery module, or battery pack can be used as a power source for the electrical device, or as an energy storage unit for the electrical device.
[0257] As the electrical device, a single battery cell, a battery module, or a battery pack can be selected according to its usage requirements.
[0258] Figure 5 shows an example of an electrical device. The electrical device disclosed in this application can be a gasoline-powered vehicle, a natural gas-powered vehicle, or a new energy vehicle. New energy vehicles can be pure electric vehicles, hybrid electric vehicles, or range-extended electric vehicles, etc. A battery device is installed inside the vehicle, and the battery device can be located at the bottom, front, or rear of the vehicle. The battery device can be used to power the vehicle; for example, the battery device can serve as the vehicle's operating power source. The vehicle may also include a controller and a motor. The controller is used to control the battery device to supply power to the motor, for example, for the vehicle's starting, navigation, and operating power needs. In some embodiments of this application, the battery device can not only serve as the vehicle's operating power source but also as the vehicle's driving power source, replacing or partially replacing gasoline or natural gas to provide driving power to the vehicle.
[0259] This application also provides an energy storage device that uses a battery as a power source. The energy storage device can be, but is not limited to, an energy storage container, an energy storage cabinet, an energy storage power station, an energy storage battery pack, or a portable energy storage system.
[0260] Example
[0261] The following describes embodiments of this application. The embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.
[0262] Example 1
[0263] (1) Preparation of positive electrode active material
[0264] Lithium carbonate, iron phosphate, titanium dioxide, vanadium pentoxide, sucrose, glucose, and polyethylene glycol were added to deionized water and mixed in a premixing tank. The ratio of lithium carbonate to iron phosphate was such that the molar ratio of lithium to iron was 1.02:1.0. Based on the total mass of the mixed raw materials, the mass content of sucrose was 2%, the mass content of glucose was 4%, and the mass content of polyethylene glycol was 5%. After uniform mixing, a mixed raw material with a solid content of 38% was obtained.
[0265] Among them, the particle size Dv of lithium carbonate 50 The particle size is 6 μm; the morphology of the iron phosphate particles is spherical; both titanium dioxide and vanadium pentoxide are nanoparticles; the purity of sucrose is ≥98%; the moisture content of glucose is <0.5%; and the weight average molecular weight of polyethylene glycol is 1500.
[0266] The mixed raw materials were ground twice in a sand mill, coarsely ground for 1 hour and then finely ground. During the grinding process, the slurry temperature was controlled to be less than 40 degrees Celsius to obtain a mixed slurry. The particle size Dv50 of the solid particles in the mixed slurry was 0.40 μm. Spray drying was then performed to obtain a dried precursor powder, and the particle size Dv50 after drying was 55.50 μm.
[0267] The precursor powder was subjected to a two-stage heating sintering process in a nitrogen atmosphere to obtain the positive electrode active material: the temperature was increased from 25℃ to 460℃ at a heating rate of 2℃ / min (first heating stage), and held for 3 hours; the temperature was then increased from 460℃ to 780℃ at a heating rate of 5℃ / min (second heating stage), and held for 12 hours; the air volume in the heating stage was greater than that in the isothermal stage, with a ratio of 1.5:1, and the total air volume was 1350 cm³. 3 / h, after which the temperature is lowered; the lithium iron phosphate cathode active material with carbon material on the surface is obtained by air jet milling with a particle size Dv50 of 1.6μm. The total mass of the cathode active material has a Ti element content of 1050ppm and a V element content of 950ppm.
[0268] The Dv10, Dv50, and Dv90 mentioned above refer to data obtained through the Malvern laser scattering method.
[0269] (2) Preparation of positive electrode sheet
[0270] The above-mentioned positive electrode active material (93.9% by mass), conductive agent (2% by mass), and binder polyvinylidene fluoride (3% by mass) were mixed in the solvent N-methylpyrrolidone. Then, dispersant HNBR (1.1% by mass) was added, and the mixture was thoroughly mixed, stirred, and dispersed in a stirring tank to form a positive electrode slurry. After the stirring process, the positive electrode slurry was transported to the coating process. The mass percentages of the positive electrode active material, conductive agent, binder, and dispersant were calculated based on the total mass of solids in the positive electrode slurry. The conductive agent included conductive carbon black (1.33% by mass) and single-walled carbon nanotubes (0.67% by mass), and the specific surface area of the conductive carbon black was 85 m². 2 / g, oil absorption value of 200ml / 100g, average length of single-walled carbon nanotubes of 30μm, specific surface area of 300m² 2 / g, the mass content of metallic impurities in single-walled carbon nanotubes is <1wt%;
[0271] The positive electrode slurry was transferred and coated onto a current collector aluminum foil, dried, and then hot-pressed to obtain a positive electrode film with a single-sided thickness of 105.64 μm and a compaction density of 2.36 g / cm³. 3 The positive electrode sheet. The transfer coating speed is 20 m / min.
[0272] The hot pressing process includes three hot roller pressing processes, with the hot roller pressing pressure increasing sequentially to 40 tons, 60 tons, and 80 tons. The hot roller temperature is 60℃. Before the first hot roller compaction, the electrode sheet is heated to 40℃.
[0273] The compaction density here refers to the compaction density of a single battery cell under full discharge conditions. The test method is described below.
[0274] Among them, the median C of the graphitization degree of the positive electrode film layer 50 The porosity of the positive electrode film is 16.1%; the iron dissolution rate of the positive electrode material is 974 ppm; the total area ratio of the agglomerated region of the conductive agent is 1.99%; and the uniformity of the distribution of particles with a diameter greater than or equal to 1 μm in the cross-section of the positive electrode film along the thickness direction of the electrode sheet is 1.85%.
[0275] The positive electrode sheets are slit and punched into specified shapes, and then the punched positive electrode sheets are sorted by weight using a weighing and sorting machine for stacking by a stacking machine.
[0276] (3) Preparation of negative electrode sheet
[0277] Natural graphite, conductive carbon black, styrene-butadiene rubber (SBR) binder, and sodium carboxymethyl cellulose (CMC) thickener are mixed evenly in a weight ratio of 95:1:2:2 and deionized water is added. After stirring and dispersing, a negative electrode slurry is obtained. The negative electrode slurry is coated on a copper foil substrate, and after drying, compaction, slitting, and sheet forming, a negative electrode sheet is obtained.
[0278] The negative electrode sheets are slit and punched into specified shapes, and then the punched negative electrode sheets are sorted by weight using a weighing and sorting machine for stacking by a stacking machine.
[0279] (4) Diaphragm
[0280] Polyvinylidene fluoride (PVDF) was dissolved in N-methylpyrrolidone (NMP) and stirred until homogeneous. Polyethylene glycol (PEG) was then added as a pore-forming agent and thoroughly mixed to obtain an adhesive layer solution. This adhesive layer solution was applied to a base film with ceramic layers on both sides. After pre-evaporation at 80°C and drying at 110°C, the film was immersed in deionized water to dissolve the PEG, resulting in a membrane with porous adhesive layers on both sides. The base film thickness was 8 μm, the ceramic layer thickness on one side was 3 μm, and the adhesive layer thickness on one side was 1 μm.
[0281] (5) Electrolyte
[0282] In an argon atmosphere glove box (H2O < 0.1 ppm, O2 < 0.1 ppm), organic solvents dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), and ethylene carbonate (EC) are mixed evenly.
[0283] Lithium hexafluorophosphate was then added and dissolved in an organic solvent to achieve a concentration of 1.05 mol / L. Ethylene carbonate (VC) was then added and stirred until homogeneous to obtain the electrolyte of Example 1.
[0284] Based on the total mass of the electrolyte, the mass content of dimethyl carbonate is 26%, the mass content of methyl ethyl carbonate is 43.3%, the mass content of ethylene carbonate is 17.3%, and the mass content of vinylene carbonate is 0.9%.
[0285] (6) Battery manufacturing
[0286] The positive electrode, separator, and negative electrode are stacked in sequence using a stacking machine. The separator must effectively isolate the positive and negative electrodes to obtain a stacked battery cell. The stacked battery cell is then coated with adhesive to ensure tight coverage. The coated stacked battery cell is placed in an outer packaging material, an aluminum-plastic film, which is composed of an inner polypropylene layer, a middle aluminum foil layer, and an outer nylon composite layer. The aluminum-plastic film outer packaging is then formed and trimmed using a punching machine to obtain the target shape and size. The aluminum-plastic film is then heat-sealed to ensure a sealing tensile strength ≥25N / 8mm. The battery undergoes vacuum baking, settling, electrolyte injection, and sealing. Finally, the soft-pack battery is subjected to hot and cold pressing operations. The hot pressing temperature is 45℃, the time is 2 minutes, and the pressure is 90kg / cm². 2 The cold pressing temperature was 25℃, the time was 2 minutes, and the pressure was 90 kg / cm². 2 Finally, after processes such as formation, vacuum degassing, and edge trimming, the battery cell is obtained. The battery cell has a length of 600mm, a width of 125mm, and a thickness of 20mm.
[0287] The preparation methods of Examples 2-3 are basically the same as those of Example 1, except that the preparation methods of the positive electrode active material and the positive electrode sheet are adjusted, as detailed below:
[0288] Example 2
[0289] The preparation method of Example 2 is basically the same as that of Example 1, except that the preparation process of the positive electrode active material and the hot pressing process of the positive electrode sheet are slightly different. The specific differences include:
[0290] (1) The carbon sources in the mixed raw materials are sucrose and glucose. The mass of sucrose is 2 wt% of the mass of iron phosphate, and the mass of glucose is 4 wt% of the mass of iron phosphate.
[0291] (2) The heating and sintering processes are different. The precursor powder is sintered at least twice in a nitrogen atmosphere. The first sintering temperature is 765℃ and the holding time is 8 hours to obtain the initial sintered product.
[0292] 1.5 wt% (based on the mass of the initial calcination product) of glucose, 3.0 wt% (based on the mass of the initial calcination product) of polyethylene glycol, titanium dioxide, and vanadium pentoxide were added to the initial calcination product. After grinding evenly, the mixture was divided into two groups for secondary grinding. The grinding parameters for the two groups were different, and the particle size distribution (D) of the particles after grinding in the first group was controlled. V 50 is 2.2μm, and the D of the particles after the second group of grinding is... V 50 represents 0.4 μm. The ground particles from the first and second groups were mixed at a mass ratio of 30:70, spray-dried, and then subjected to a second sintering. The second sintering temperature was 815℃, and the temperature was maintained for 10 hours.
[0293] Based on the total mass of the positive electrode active material, the mass content of Ti is 1050 ppm and the mass content of V is 950 ppm.
[0294] (3) The positive electrode slurry was transferred and coated onto the current collector aluminum foil, dried, and hot-pressed to obtain a positive electrode film with a single-sided thickness of 106.34 μm and a compaction density of 2.37 g / cm³. 3 The positive electrode sheet. The drying temperature is 95℃ and the drying speed is 2.0m / min.
[0295] The hot pressing process includes three hot rolling processes, with the hot rolling pressure increasing sequentially to 35 tons, 55 tons, and 70 tons. The hot rolling temperature is 65℃. Before the first hot rolling compaction, the electrode sheet is heated to 50℃. The compaction density here refers to the compaction density of the battery cell under full discharge conditions, and its testing method is described below.
[0296] Example 3
[0297] The preparation method of Example 3 is basically the same as that of Example 1, except that the sintering process of the positive electrode active material and the hot pressing process of the positive electrode sheet are different. Specifically:
[0298] (1) The precursor powder is subjected to two-stage heating and sintering in a nitrogen atmosphere to obtain the positive electrode active material: the temperature is increased from 25℃ to 440℃ at a heating rate of 2℃ / min (first heating stage) and held for 2.5h; the temperature is increased from 440℃ to 760℃ at a heating rate of 5℃ / min (second heating stage) and held for 11h; and then the airflow pulverization intensity is increased to obtain the lithium iron phosphate positive electrode active material with carbon material on the surface.
[0299] (2) The positive electrode slurry was transferred and coated onto the current collector aluminum foil, dried, and hot-pressed to obtain a positive electrode film with a single-sided thickness of 105.65 μm and a compaction density of 2.36 g / cm³. 3 The positive electrode sheet. The transfer coating speed is 20 m / min.
[0300] The hot pressing process includes three hot roller pressing processes, with the hot roller pressing pressure increasing sequentially to 45 tons, 60 tons, and 80 tons. The hot roller temperature is 60℃. Before the first hot roller compaction, the electrode sheet is heated to 40℃.
[0301] The preparation methods of Examples 4-8 are basically the same as those of Example 1, except that the preparation method of the positive electrode sheet is adjusted, as follows:
[0302] Example 4
[0303] The positive electrode slurry from Example 1 was transferred and coated onto a current collector aluminum foil and dried. By adjusting the pressure, rolling speed, roll gap, holding time, number of rolling passes, and controlling the coating density in the hot pressing process, a positive electrode sheet with a single-sided thickness of 91.88 μm was obtained through hot pressing; the compaction density of the positive electrode sheet was 2.36 g / cm³. 3 The compaction density here refers to the compaction density of a single battery cell under full load. The testing method is described below. Keeping the number of layers constant, the thickness of the battery cell is adjusted adaptively according to the thickness of the positive electrode film.
[0304] Example 5
[0305] The positive electrode slurry from Example 1 was transferred and coated onto a current collector aluminum foil and dried. By adjusting the pressure, rolling speed, roll gap, holding time, number of rolling passes, and controlling the coating density in the hot pressing process, a positive electrode sheet with a single-sided thickness of 116.09 μm was obtained through hot pressing; the compaction density of the positive electrode sheet was 2.36 g / cm³. 3 The compaction density here refers to the compaction density of a single battery cell under full load. The testing method is described below. Keeping the number of layers constant, the thickness of the battery cell is adjusted adaptively according to the thickness of the positive electrode film.
[0306] Example 6
[0307] The positive electrode slurry from Example 1 was transferred and coated onto a current collector aluminum foil and dried. By adjusting the pressure, rolling speed, roll gap, holding time, number of rolling passes, and controlling the coating density in the hot pressing process, a positive electrode sheet with a single-sided thickness of 72.34 μm was obtained through hot pressing; the compaction density of the positive electrode sheet was 2.36 g / cm³. 3 The compaction density here refers to the compaction density of a single battery cell under full load. The testing method is described below. Keeping the number of layers constant, the thickness of the battery cell is adjusted adaptively according to the thickness of the positive electrode film.
[0308] Example 7
[0309] The positive electrode slurry from Example 1 was transferred and coated onto a current collector aluminum foil and dried. By adjusting the pressure, rolling speed, roll gap, holding time, number of rolling passes, and controlling the coating density in the hot pressing process, a positive electrode sheet with a single-sided thickness of 83.91 μm was obtained through hot pressing; the compaction density of the positive electrode sheet was 2.36 g / cm³. 3 The compaction density here refers to the compaction density of a single battery cell under full load. The testing method is described below. Keeping the number of layers constant, the thickness of the battery cell is adjusted adaptively according to the thickness of the positive electrode film.
[0310] Example 8
[0311] The positive electrode slurry from Example 1 was transferred and coated onto a current collector aluminum foil and dried. By adjusting the pressure, rolling speed, roll gap, holding time, number of rolling passes, and controlling the coating density in the hot pressing process, a positive electrode sheet with a single-sided thickness of 98.93 μm was obtained through hot pressing; the compaction density of the positive electrode sheet was 2.52 g / cm³. 3 The compaction density here refers to the compaction density of a single battery cell under full load. The testing method is described below. Keeping the number of layers constant, the thickness of the battery cell is adjusted adaptively according to the thickness of the positive electrode film.
[0312] Example 9
[0313] The preparation method of Example 9 is basically the same as that of Example 1, except that the preparation methods of the positive electrode active material and the positive electrode sheet are adjusted, as detailed below:
[0314] First, a precursor solution was prepared under argon protection by mixing FeSO4·7H2O, LiOH·H2O, and H3PO4 in deionized water, and adding 0.5wt% ascorbic acid as an antioxidant. Then, the pH was adjusted to 5.0, and 0.1mol / L citric acid was added as a grain growth inhibitor and 1wt% PEG-4000 as a dispersant. The mixed solution was transferred to a high-pressure reactor and reacted at 180℃ for 6 hours. After centrifugation and washing, the reaction product was vacuum dried at 80℃ and finally annealed at 350℃ in an argon atmosphere for 2 hours to obtain lithium iron phosphate material with an average particle size of 160nm.
[0315] The lithium iron phosphate material prepared above was mixed with the positive electrode active material of Example 1 at a mass ratio of 10:90 to obtain the positive electrode active material of Example 9.
[0316] The positive electrode slurry was transferred and coated onto the current collector aluminum foil and dried. By adjusting the pressure, rolling speed, roll gap, holding time, and number of rolling passes in the hot pressing process, and controlling the coating density, a positive electrode sheet with a single-sided thickness of 105.65 μm was obtained through hot pressing; the compaction density of the positive electrode sheet was 2.36 g / cm³.3 The compaction density here refers to the compaction density of a single battery cell under full load. The testing method is described below. Keeping the number of layers constant, the thickness of the battery cell is adjusted adaptively according to the thickness of the positive electrode film.
[0317] Example 10
[0318] The preparation method of Example 10 is basically the same as that of Example 9, except that the preparation method of the positive electrode sheet is adjusted, as follows:
[0319] The positive electrode active material of Example 9 was prepared using the same positive electrode preparation method as in Example 1, resulting in a positive electrode sheet with a single-sided thickness of 105.65 μm and a compaction density of 2.32 g / cm³. 3 The compaction density here refers to the compaction density of a single battery cell under full discharge conditions. The test method is described below.
[0320] The preparation method of Comparative Example 1 is basically the same as that of Example 1, except that the preparation method of the positive electrode active material is adjusted, as follows:
[0321] Comparative Example 1
[0322] The preparation method of Comparative Example 1 is basically the same as that of Example 1, except that the sintering process of the positive electrode active material is different, specifically:
[0323] The precursor powder was subjected to a two-stage heating and sintering process in a nitrogen atmosphere to obtain the positive electrode active material: the temperature was increased from 25℃ to 500℃ at a heating rate of 2℃ / min (first heating stage) and held for 3.5h; the temperature was increased from 500℃ to 800℃ at a heating rate of 5℃ / min (second heating stage) and held for 13h; after reducing the airflow pulverization intensity, the lithium iron phosphate positive electrode active material with carbon material on the surface was obtained.
[0324] The preparation method of Comparative Example 2 is basically the same as that of Example 1, except that the preparation method of the positive electrode active material is adjusted, as follows:
[0325] Comparative Example 2
[0326] First, a precursor solution was prepared under argon protection by mixing FeSO4·7H2O, LiOH·H2O, and H3PO4 in deionized water, and adding 0.5wt% ascorbic acid as an antioxidant. Then, the pH was adjusted to 5.0, and 0.1mol / L citric acid was added as a grain growth inhibitor and 1wt% PEG-4000 as a dispersant. The mixed solution was transferred to a high-pressure reactor and reacted at 180℃ for 6 hours. After centrifugation and washing, the reaction product was vacuum dried at 80℃ and finally annealed at 350℃ in an argon atmosphere for 2 hours to obtain lithium iron phosphate material with an average particle size of 160nm.
[0327] The lithium iron phosphate material prepared above was mixed with the positive electrode active material of Example 1 at a mass ratio of 12:88 to obtain the positive electrode active material of Comparative Example 2.
[0328] It is understood that the positive electrode preparation processes of Examples 1, 10 and Comparative Example 2 are the same; however, Examples 9 and 10 use the same positive active material preparation process but have different positive electrode preparation processes.
[0329] Test method:
[0330] 1. Capacity of a single battery cell
[0331] At 25℃, charge the battery cell to 3.65V at a charging rate of 0.5C (the nominal capacity of the single cell), then charge it to 0.05C at a constant voltage of 3.65V, let it stand for 10 minutes, and then discharge it to 2.5V at a discharge rate of 1C, let it stand for 10 minutes. Calculate the capacity C during the discharge process using the formula C=I*t, with the unit being Ah.
[0332] 2. Number of cycles corresponding to 85% capacity decay
[0333] At 25°C, charge the battery cell to 3.65V at a charging rate of 0.5C (the nominal capacity of the single cell), then charge it to 0.05C at 3.65V, let it stand for 10 minutes, and then discharge it to 2.5V at a discharging rate of 1C, let it stand for 10 minutes. One charge-discharge cycle is one cycle. Continue the test until the battery capacity decays to 85% of the nominal capacity. This number of cycles is recorded as the number of cycles @ 85% SOH.
[0334] Test Results
[0335] Table 1
[0336] As can be seen from the comparison of the examples and comparative examples, in the cross-section of the positive electrode film along the thickness direction of the electrode sheet, the area ratio of particles with a diameter greater than or equal to 1 μm is 12%-50%, and the area ratio of particles with a diameter greater than 50 nm and less than or equal to 200 nm is 3.0%-15.0%. Under full discharge conditions, the compaction density of the positive electrode sheet is 2.3 g / cm³. 3 -2.6g / cm 3 At the same time, the battery cells maintain good capacity while mitigating stress concentration caused by large particles during electrode compaction. The positive electrode film has low resistivity, improving the battery's cycle performance and dynamic performance.
[0337] As can be seen from the comparison between Example 2 and Examples 1 and 3, in the cross section of the positive electrode film along the thickness direction of the electrode sheet, the area ratio of particles with a diameter greater than or equal to 1 μm is 12%-40%. This is beneficial for the battery to maintain high capacity, further improve the stress concentration phenomenon of large particles during the electrode sheet compaction process, reduce the probability of film loosening and active material shedding, and improve the cycle performance of the battery.
[0338] As can be seen from the comparison between Example 9 and Examples 1-3, in the cross-section of the positive electrode film along the thickness direction of the electrode sheet, the area ratio of particles with a diameter greater than 50nm and less than or equal to 200nm is 5%-10%, which is beneficial for the battery to reduce the resistivity of the positive electrode film and improve the dynamic performance of the battery while maintaining high capacity and good cycle performance.
[0339] A comparison of Example 5 with Examples 1-4 and 6-9 shows that, in the cross-section of the positive electrode film along the electrode thickness direction, the median L of the sphericity in the cumulative distribution curve of the sphericity area of particles with a diameter greater than or equal to 1 μm is... A50 The value is 0.67-0.75, which further improves the stress concentration phenomenon that occurs during the compaction of large particles in the electrode sheet, reduces the probability of film loosening and active material shedding, and improves the cycle performance of the battery.
[0340] As can be seen from the comparison of Examples 6 and 7 with Examples 4 and 5, the single-sided thickness of the positive electrode film is 90μm-120μm, which is beneficial to further improve the battery capacity.
[0341] It should be noted that this application is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this application are included in the technical scope of this application. Furthermore, various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing by combining some of the constituent elements of the embodiments, without departing from the spirit of this application, are also included in the scope of this application.
Claims
1. A battery cell, characterized by, comprising a laminated cell, the laminated cell comprising a positive electrode plate and a negative electrode plate, the positive electrode plate comprising a positive current collector and a positive electrode film layer disposed on at least one side of the positive current collector, the positive electrode film layer comprising lithium-containing transition metal phosphate particles, at least part of the surface of the lithium-containing transition metal phosphate particles being provided with a carbon material; in the cross section of the positive electrode film layer along the thickness direction of the electrode plate, the area proportion of particles with a particle diameter of 1 μm or more is 12%-50%; in the cross section of the positive electrode film layer along the thickness direction of the electrode plate, the area proportion of particles with a particle diameter of more than 50 nm and 200 nm or less is 3.0%-15.0%; The battery cell in full discharge state, the compaction density of the positive pole piece is 2.3g / cm 3 -2.6g / cm 3 .
2. The battery cell of claim 1, wherein, in the cross section of the positive electrode film layer along the thickness direction of the electrode plate, the area proportion of particles with a particle diameter of 1 μm or more and 5 μm or less is 12%-50%, optionally 12%-40%.
3. The battery cell according to claim 1 or 2, characterized in that, in the cross section of the positive electrode film layer along the thickness direction of the electrode plate, the distribution uniformity of particles with a particle diameter of 1 μm or more is 0.2%-5%, optionally 0.2%-2%.
4. The battery cell of any one of claims 1-3, wherein, In a section of the positive electrode film layer along the thickness direction of the electrode tab, in a cumulative distribution curve of the sphericity of particles with a particle size of 1 μm or more, the median L of the sphericity is 0.6-0.8, optionally 0.65-0.75, further optionally 0.67-0.
75. A50 In a section of the positive electrode film layer along the thickness direction of the electrode tab, in a cumulative distribution curve of the sphericity of particles with a particle size of 1 μm or more, the median L of the sphericity is 0.6-0.8, optionally 0.65-0.75, further optionally 0.67-0.
75.
5. The battery cell of any one of claims 1-4, wherein, in the cross section of the positive electrode film layer along the thickness direction of the electrode plate, the area proportion of particles with a particle diameter of more than 50 nm and 200 nm or less is 5.0%-15.0%, optionally 5.0%-10.0%.
6. The battery cell of any one of claims 1-5, wherein, The single-side thickness of the positive electrode film layer is 70 μm-120 μm, optionally 90 μm-120 μm, further optionally 100 μm-120 μm.
7. The battery cell of any one of claims 1-6, wherein, The positive electrode film layer further comprises a conductive agent, and based on the total area of the cross section of the positive electrode film layer along the thickness direction of the electrode plate, the total area proportion of agglomerated regions of the conductive agent is 0.2%-6%, optionally 1.5%-5%.
8. The battery cell of claim 7, wherein, The conductive agent comprises carbon nanotubes, and the carbon nanotubes comprise one or more of single-walled carbon nanotubes, few-walled carbon nanotubes and multi-walled carbon nanotubes, optionally, the conductive agent further comprises conductive carbon black.
9. The battery cell according to claim 7 or 8, characterized in that, The agglomerated regions of the conductive agent comprise carbon nanotubes and conductive carbon black.
10. The battery cell of claim 9, wherein, Based on the mass of the positive electrode film layer, the mass content C1 of the carbon nanotubes satisfies: 0<C1≤2.5%, and the mass content C2 of the conductive carbon black satisfies: 0<C2≤2.5%.
11. The battery cell of any one of claims 1-10, wherein, The positive electrode film layer further comprises a dispersant, and the dispersant comprises hydrogenated nitrile butadiene rubber (HNBR).
12. The battery cell of claim 11, wherein, Based on the mass of the positive electrode film layer, the mass content of the dispersant is 0.5%-2%.
13. The battery cell of any one of claims 1-12, wherein, A primer layer is disposed in the bottom region of the positive electrode film layer close to the positive current collector, and the primer layer satisfies at least one of the following conditions: (1) The primer layer comprises a conductive agent and a binder, the conductive agent comprises carbon nanotubes and conductive carbon black, and the binder comprises a vinylidene fluoride polymer; (2) The thickness of the primer layer is 0.5 μm-5 μm.
14. The battery cell of any one of claims 1-13, wherein, The median value C of graphitization degree in a cumulative distribution curve of graphitization degree C value obtained by the positive electrode film layer in a laser microscopic confocal Raman spectrometer face scanning mode 50 greater than or equal to 0.95 and less than or equal to 1.20; wherein the graphitization degree C value is I G / I D , I G represents the G peak intensity of the Raman spectrum at 1580±100 cm -1 , I D represents the D peak intensity of the Raman spectrum at 1350±100 cm -1 .
15. The battery cell of any one of claims 1-14, wherein, The lithium-containing transition metal phosphate particles in the positive electrode film layer include a component represented by the following general formula: Li m Fe x P y O j Q q Formula I, Herein, Q comprises one or more of Al, Na, K, Mg, Cu, Mn, Cr, Zn, Pb, Ca, Co, Ni, Sr, Nb, V, Ti, B, S, Si, N, F, Cl, Br, 0.8≤m≤1.15, 0.9≤x≤1, 0.95≤y≤1, 3.5≤j≤4, 0≤q≤0.
1.
16. The battery cell of any one of claims 1-15, wherein, The lithium-containing transition metal phosphate particles include titanium. Based on the total mass of the lithium-containing transition metal phosphate particles in the positive electrode film, the mass content of titanium is 500ppm-8000ppm, and can be selected as 1000ppm-3000ppm.
17. The battery cell of any one of claims 1-16, wherein, The lithium-containing transition metal phosphate particles include vanadium. Based on the total mass of the lithium-containing transition metal phosphate particles in the positive electrode film, the mass content of vanadium is 500ppm-5000ppm, and can be selected as 500ppm-3000ppm.
18. The battery cell of any one of claims 1-17, wherein, The porosity of the positive electrode film is 14%-28%.
19. The battery cell of any one of claims 1-18, wherein, The resistivity of the positive electrode film is 10 Ω·cm-35 Ω·cm.
20. The battery cell of any one of claims 1-19, wherein, The battery cell further includes a separator disposed between the positive electrode and the negative electrode. The separator includes a base film, ceramic layers disposed on both sides of the base film, and an adhesive layer disposed on at least one side of the ceramic layer away from the base film. The adhesive layer is a continuous layer with a porous structure and includes a vinylidene fluoride polymer.
21. The battery cell of any one of claims 1-20, wherein, The battery cell includes a housing, and the stacked cells are housed within the housing. The housing has a length dimension of L0, a width dimension of W0, and a thickness dimension of H0, with the following dimensions: 450mm≤L0≤1300mm, 100mm≤W0≤150mm, and 14mm≤H0≤22mm.
22. The battery cell of claim 21, wherein, The length dimension L0 of the shell satisfies: 450mm≤L0≤650mm.
23. The battery cell of claim 21, wherein, The length dimension L0 of the shell satisfies: 900mm≤L0≤1300mm.
24. The battery cell of any one of claims 20-23, wherein, The housing satisfies at least one of the following conditions: (1) The material of the shell is a soft-pack material, which includes an aluminum-plastic composite film, and optionally includes one or more of polypropylene (PP), polybutylene terephthalate (PBT), polybutylene succinate (PBS), nylon, polyethylene terephthalate (PET), and polyethylene (PE) to form a composite film with aluminum. (2) The housing includes a first sealing area, which is disposed at at least one end of the laminated cell extending in the width direction; the first sealing area includes a folded edge structure extending in the length direction, and the folded edge structure is provided with encapsulating adhesive, which is continuously disposed in the length direction and fixes the folded edge structure. (3) The housing includes at least one second sealing area, which is disposed at at least one end of the laminated cell along the length direction of the housing, and the second sealing area is disposed on the tab side of the laminated cell.
25. The battery cell of any one of claims 1-24, wherein, The outer periphery of the laminated battery cell is provided with a plurality of rubber rings that surround it along the width direction, and the rubber rings that surround it along the width direction are spaced apart along the length direction.
26. The battery cell of any one of claims 1-25, wherein, At 25°C, the capacity of the battery cell is 100Ah-300Ah, optionally 110Ah-190Ah, and further optionally 125Ah-180Ah.
27. A battery device, characterized by Includes the battery cell as described in any one of claims 1-26.
28. An electrical device, comprising: The electrical device includes the battery device as described in claim 27, the battery device being used to provide electrical energy.
29. An energy storage device, comprising: The energy storage device includes the battery device of claim 27 for storing electrical energy.