Battery cell, battery device, electric device and energy storage device

By optimizing the stacked cell structure and positive electrode design, and combining materials such as carbon nanotubes and conductive carbon black, the problem of balancing capacity and cycle performance in lithium-ion secondary batteries has been solved, achieving high capacity and long lifespan battery performance.

WO2026236905A1PCT designated stage Publication Date: 2026-11-19CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2025/094409
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2025-05-12
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing technologies make it difficult to simultaneously improve the capacity and cycle performance of lithium-ion secondary batteries, resulting in a trade-off between high capacity and good cycle performance.

Method used

By adopting a stacked cell structure and increasing the compaction density of the positive electrode sheet, the risk of film detachment is reduced by adjusting the median graphitization degree C₅₀ and controlling the particle slippage ability of the positive electrode film. The internal structure of the battery is optimized by combining materials such as carbon nanotubes and conductive carbon black to form a uniform conductive network.

Benefits of technology

This achieves an effective balance between high capacity and good cycle performance, improving the battery's volumetric energy density and cycle life, while reducing the risk of film shedding and internal resistance, and improving the battery's dynamic performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2025094409_19112026_PF_FP_ABST
    Figure CN2025094409_19112026_PF_FP_ABST
Patent Text Reader

Abstract

A battery cell, a battery device, an electric device, and an energy storage device. The battery cell comprises a stacked cell, wherein the stacked cell comprises a positive electrode sheet and a negative electrode sheet; the positive electrode sheet comprises a positive electrode current collector and a positive electrode film layer arranged on at least one side of the positive electrode current collector; the positive electrode film layer comprises lithium-containing transition metal phosphate particles, at least a portion of the surface of each of which is provided with a carbon material; in a cumulative distribution curve of graphitization degree C values of the positive electrode film layer obtained in an area scanning mode of a laser confocal Raman microscope, the median C50 of the graphitization degree is 0.95-1.20, wherein the graphitization degree C value is IG / ID, IG represents the G-peak intensity of the Raman spectrum at 1580±100 cm-1, and ID represents the D-peak intensity of the Raman spectrum at 1350±100 cm-1. When the battery cell is in a fully discharged state, the compaction density of the positive electrode sheet is 2.3 g / cm3 to 2.6 g / cm3. The battery cell has both high capacity and good cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Battery cells, battery devices, electrical devices, and energy storage devices Technical Field

[0001] This application relates to the field of lithium-ion secondary battery cell technology, and in particular to a battery cell, battery device, power supply device, and energy storage device. Background Technology

[0002] In recent years, lithium-ion rechargeable battery cells have been widely used in energy storage power systems such as hydropower, thermal power, wind power and solar power plants, as well as in many fields such as power tools, electric bicycles, electric motorcycles, electric cars, military equipment, and aerospace.

[0003] As the market demands longer driving range and longer battery life, higher requirements are being placed on battery capacity and cycle performance. However, current technologies struggle to simultaneously improve these performance aspects, making it crucial to address this critical technical challenge. Summary of the Invention

[0004] This application is made in view of the above-mentioned issues, and its purpose is to provide a battery cell that has both high capacity and good cycle performance.

[0005] The first aspect of this application provides a battery cell comprising a stacked cell, the stacked cell comprising a positive electrode and a negative electrode, the positive electrode comprising a positive current collector and a positive electrode film disposed on at least one side of the positive current collector, the positive electrode film comprising lithium transition metal phosphate particles of carbon material disposed on at least a portion of its surface, and the median C of the graphitization degree C value of the positive electrode film obtained in the laser microscopy confocal Raman spectroscopy instrument scanning mode. 50 The value ranges from 0.95 to 1.20, where the degree of graphitization C is I. G / I D I G This indicates that the Raman spectrum is at 1580±100 cm⁻¹ -1 The intensity of peak G at I D This indicates that the Raman spectrum is at 1350±100 cm⁻¹ -1 The intensity of peak D at the specified location indicates that, under fully discharged conditions, the compaction density of the positive electrode sheet is 2.3 g / cm³. 3 -2.6g / cm 3 .

[0006] This application reduces the ineffective space inside the battery cell and improves space utilization by adopting a stacked cell structure and increasing the compaction density of the positive electrode sheet, thereby improving the volumetric energy density and capacity of the battery cell, while simultaneously controlling the median graphitization degree C. 50(Reflecting the degree of order of carbon coating materials), reducing frictional resistance between particles, enhancing the ability of particles to slide in the positive electrode film, reducing stress concentration in the positive electrode film, reducing the risk of film shedding during cycling, and ultimately achieving an effective balance between high capacity and good cycle performance in the battery.

[0007] In any embodiment, the median C of the graphitization degree C value in the cumulative distribution curve of the positive electrode film obtained in the laser microscopy confocal Raman spectroscopy instrument scanning mode is... 50 The value is 1.01-1.13.

[0008] When the graphitization degree of the positive electrode film is within the above range, it helps to further improve the slippage ability of particles in the positive electrode film, reduce stress concentration in the positive electrode film, reduce the risk of film shedding during cycling, and thus further improve the cycle life of the battery cell.

[0009] In any embodiment, based on the total area of ​​particles in the cross section along the thickness direction of the positive electrode film, the area ratio of particles with a particle size R1 satisfying R1≥1000nm is 12%-50%, and can be selected as 12%-40%.

[0010] In the cross-section of the positive electrode film along the thickness direction of the electrode sheet, the area ratio of particles with a particle size R1 satisfying R1≥1000nm is in the range of 12%-50%, and further in the range of 12%-40%. This can improve the compaction density of the electrode sheet without increasing the probability of film shedding, thereby improving the energy density of the battery cell, alleviating the capacity drop problem, and taking into account the cycle life of the battery.

[0011] In any embodiment, in the cross-section of the positive electrode film along the electrode thickness direction, in the cumulative distribution curve of the particle spheroidity area where the particle size R1 satisfies R1≥1000nm, the median L of the spheroidity is... R1A1 50 is 0.6-0.8, can be selected as 0.65-0.75, and can be further selected as 0.67-0.75.

[0012] In the cross-section of the positive electrode film along the thickness direction of the positive electrode sheet, in the cumulative area distribution curve of the spheroidal area of ​​particles with a particle size R1 satisfying R1≥1000nm, L R1A50 Within the range of 0.65-0.75, and further within the range of 0.67-0.75, it is beneficial to further reduce stress concentration at large particles in the positive electrode film of the stacked cell, thereby reducing the probability of film peeling and improving the cycle life of the battery.

[0013] In any embodiment, the median B of the coating value B in the cumulative distribution curve of the positive electrode film obtained in the laser microscopy confocal Raman spectroscopy instrument scanning mode is... 50The value is 0.30-0.60, where the coating value B is I. P / I D , where I P This indicates that the Raman spectrum is at 948±100 cm⁻¹ -1 The intensity of the P peak at I D This indicates that the Raman spectrum is at 1350±100 cm⁻¹ -1 The intensity of peak D at that location.

[0014] The median B of the coating value of the positive electrode film 50 Within the aforementioned range, it is evident that the carbon coating material of the positive electrode active material is relatively dense and uniform, which is beneficial for improving the slip uniformity of the positive electrode film during the rolling process and reducing stress concentration in the positive electrode film. In addition, thanks to the dense and uniform carbon coating material, large particles in the positive electrode film are more likely to slip during the compaction process, thereby reducing stress concentration at large particles in the positive electrode film, reducing the probability of film detachment, improving the problem of battery capacity drop, and increasing the cycle life of the battery.

[0015] In any embodiment, the lithium-containing transition metal phosphate particles comprise components represented by the following general formula: Li m Fe x P y O j Q q Formula I,

[0016] Wherein, Q includes one or more of Al, Na, K, Mg, Cu, Mn, Cr, Zn, Pb, Ca, Co, Ni, Sr, Nb, V, Ti, B, S, Si, N, F, Cl, and Br, with 0.8≤m≤1.15, 0.9≤x≤1, 0.95≤y≤1, 3.5≤j≤4, and 0≤q≤0.1.

[0017] In any embodiment, the lithium-containing transition metal phosphate particles in the positive electrode film layer include one or more of lithium iron phosphate, lithium manganese phosphate, lithium fluorinated vanadium phosphate, lithium manganese iron phosphate, and their modified materials.

[0018] In any embodiment, the lithium-containing transition metal phosphate particles in the positive electrode film layer include one or more of lithium iron phosphate and its doped and modified materials, and coating and modified materials.

[0019] In any embodiment, the iron dissolution rate of the positive electrode active material is 658ppm-1921ppm, and can be selected as 658ppm-1485ppm.

[0020] In any embodiment, the mass content of titanium is 500ppm-8000ppm, optionally 1000ppm-3000ppm, based on the total mass of the lithium transition metal phosphate particles.

[0021] In this embodiment, by adding a high content of titanium to lithium transition metal phosphate particles, the reactivity of the raw materials for synthesizing the positive electrode active material is reduced. This allows the positive electrode active material to achieve a high degree of graphitization while controlling the proportion of large particles, reducing stress concentration in the positive electrode film, lowering the probability of film shedding, and improving battery energy density while also considering battery cycle life.

[0022] In any embodiment, based on the total mass of lithium transition metal phosphate particles in the positive electrode film, the vanadium content is 500ppm-5000ppm, optionally 500ppm-3000ppm.

[0023] Vanadium in the positive electrode film can be in multiple valence states, including +5 vanadium (V5). 5+ Vanadium (V+3) can be doped into phosphorus sites. Due to its large radius, it can cause lattice distortion, expand the diffusion channels of lithium ions, thereby improving the ionic conductivity of the positive electrode active material and enhancing the kinetic performance of the battery; 3+ Vanadium can be doped into transition metal sites, generating lithium vacancies through charge compensation, thereby improving the electronic conductivity of the positive electrode active material. Furthermore, the increased uniformity of vanadium distribution in lithium-containing transition metal phosphate particles helps to further improve the kinetic performance and reaction uniformity of the positive electrode film, thus further enhancing the kinetic and cycle performance of the battery cell.

[0024] In any embodiment, the porosity of the positive electrode film is 14%-28%.

[0025] When the porosity of the positive electrode film is within the aforementioned range, the film exhibits good electrolyte wettability and tortuosity, which facilitates the diffusion of lithium ions between the liquid and solid phases. This helps reduce concentration polarization in thick electrodes and improves the battery's kinetic performance. Simultaneously, it helps alleviate the volume expansion of the positive electrode during cycling, reduces mechanical stress in the film, and minimizes stress concentration, thereby reducing the risk of film detachment.

[0026] In any embodiment, the resistivity of the positive electrode film is 10 Ω·cm to 35 Ω·cm.

[0027] Having the resistivity of the positive electrode film within the above range is beneficial for reducing electron transport impedance, minimizing charge-discharge polarization, and improving the rate performance and cycle performance of the battery.

[0028] In any embodiment, the thickness of the positive electrode film layer on one side is denoted as H, where H is 70μm-120μm.

[0029] In any embodiment, the thickness of the positive electrode film layer on one side is denoted as H, where H is 90μm-120μm.

[0030] Having a single-sided thickness of the positive electrode film within the above range helps to increase the loading of positive electrode active materials in the battery, thereby increasing the battery capacity, while also reducing the risk of film shedding during cycling.

[0031] In any embodiment, the thickness of the positive electrode film layer on one side is denoted as H, where H is 100μm-120μm.

[0032] Increasing the thickness of the positive electrode film helps to increase the loading of the positive electrode active material and thus improves the battery capacity. However, the applicant has found that when the single-sided thickness of the positive electrode film is greater than or equal to 100 μm, the volume expansion of the positive electrode film is more significant during battery cycling, resulting in greater stress. This leads to more pronounced stress concentration in the positive electrode film, increasing the risk of film detachment and consequently affecting the battery's cycle performance. The embodiments of this application increase the battery capacity by increasing the thickness of the positive electrode film, while simultaneously controlling the median C of the graphitization degree C value in the cumulative distribution curve obtained under laser microscopy confocal Raman spectroscopy surface scanning mode. 50 This improves the slippage ability between particles in the positive electrode film, thereby helping to reduce stress concentration in the film, reducing the risk of film shedding, and thus improving the cycle life of the battery.

[0033] In any embodiment, the positive electrode film layer has a base coating layer in the bottom region near the positive electrode current collector. The base coating layer includes a conductive agent and a binder. The conductive agent includes carbon nanotubes and conductive carbon black, and the binder includes vinylidene fluoride polymer.

[0034] In any embodiment, the thickness of the base coating is 0.5 μm to 5 μm.

[0035] The undercoating layer provided in this application helps improve the adhesion between the positive electrode film and the positive electrode current collector and alleviates stress concentration at large particles, thereby reducing the probability of positive electrode film detachment and improving the cycle stability of the battery. Simultaneously, compared to direct contact between the positive electrode current collector and the positive electrode film, the increased contact area between the undercoating layer and the positive electrode film helps increase the area for electron transport between the current collector and the positive electrode film, thereby reducing the internal resistance of the electrode and improving the battery's dynamic performance.

[0036] In any embodiment, the positive electrode film layer further includes a dispersant, the dispersant including hydrogenated nitrile butadiene rubber (HNBR).

[0037] When HNBR adsorbs onto the surface of particles in the slurry, its long-chain molecules form a physical barrier around the particles, preventing them from approaching each other and agglomerating, thus maintaining a relatively independent dispersion. Simultaneously, HNBR reduces the surface tension between the dispersion medium and the dispersed particles, making the particles easier to wet and promoting dispersion. It also reduces the interfacial energy between particles, minimizing aggregation driven by interfacial energy. Furthermore, during slurry drying and film formation, the elastic network structure of HNBR buffers the shrinkage stress caused by solvent evaporation, reducing the re-agglomeration of conductive agents due to capillary forces, lowering the area of ​​agglomerated regions, and improving the battery's kinetic performance and cycle life.

[0038] In any embodiment, the mass content of the dispersant is 0.5%-2% based on the mass of the positive electrode film.

[0039] When the mass content of the dispersant is within the above range, it can achieve uniform dispersion of particles in the positive electrode film while maintaining a high loading capacity, reduce stress concentration in the positive electrode film, effectively alleviate the problem of battery capacity drop, and improve the cycle performance of the battery.

[0040] In any embodiment, the positive electrode film layer further includes a conductive agent, and the area ratio of the agglomerated region of the conductive agent is 0.5%-2.5%, optionally 1.5%-2.5%, based on the total area of ​​the cross section of the positive electrode film layer along the thickness direction of the electrode sheet.

[0041] Based on the total area of ​​the cross-section of the positive electrode film along the thickness direction of the electrode sheet, the area ratio of the agglomeration region of the conductive agent is within the above range, indicating that the conductive agent in the positive electrode film is uniformly dispersed and it is easy to form a uniform conductive network. This is especially beneficial to reduce the problem of decreased kinetics caused by the growth of ion transport paths in the film, reduce local polarization and even lithium plating problems generated during battery cycling, and improve the cycle life of the battery.

[0042] In any embodiment, the conductive agent comprises carbon nanotubes, which include one or more of single-walled carbon nanotubes, few-walled carbon nanotubes, and multi-walled carbon nanotubes.

[0043] Due to the one-dimensional structure of carbon nanotubes, they can form a network structure in the positive electrode film layer. On the one hand, the high elastic modulus of carbon nanotubes enables their network structure not only to act as a bridge for stress propagation, but also to exert a binding effect on the positive electrode film layer, inhibit the rebound of lithium-containing transition metal phosphate particles, effectively alleviate stress concentration, reduce the risk of film layer peeling, and thus ameliorate the battery capacity diving problem; on the other hand, the excellent electrical conductivity of carbon nanotubes makes their network structure an efficient electron transmission channel. Even if local film layer peeling occurs, the thick electrode sheet can still maintain high electron transmission efficiency in the in-plane direction and the thickness direction, thereby delaying the occurrence of the capacity diving problem, and further improving the kinetic performance and cycle life of the battery.

[0044] In any embodiment, the conductive agent further comprises conductive carbon black.

[0045] Conductive carbon black has a relatively high specific surface area, and thus has good liquid retention capability. The expansion force of the thick electrode sheet during cycling is large, which makes the electrolyte easy to be squeezed out. The distribution of conductive carbon black in the positive electrode film layer is beneficial to improving the liquid retention capability of the thick electrode sheet, further alleviating the phenomenon of capacity diving of the battery during cycling, and improving the cycle life of the battery.

[0046] In any embodiment, based on the mass of the positive electrode film layer, the mass content C1 of carbon nanotubes satisfies: 0<C1≤2.5%, and the mass content C2 of conductive carbon black satisfies: 0<C2≤2.5%.

[0047] When the mass contents of carbon nanotubes and conductive carbon black are within the above ranges, the agglomeration of carbon nanotubes can be effectively alleviated and a good conductive network structure can be formed, so as to effectively reduce the stress concentration of the positive electrode film layer, increase the liquid retention rate of the positive electrode sheet during long-term cycling, further reduce the risk of electrode sheet film layer peeling and the degree of polarization, improve the kinetic performance of the battery, take into account the capacity diving problem, and ameliorate the cycle life of the battery.

[0048] In any embodiment, the battery cell comprises a housing, at least one of the laminated cores is accommodated in the housing, the dimension of the housing in the length direction is L0, the dimension of the housing in the width direction is W0, and the dimension of the housing in the thickness direction is H0, where 450mm≤L0≤1300mm, 100mm≤W0≤150mm, and 14mm≤H0≤22mm.

[0049] In any embodiment, the dimension L0 of the housing in the length direction satisfies: 450mm≤L0≤650mm.

[0050] When the length dimension L1 of the casing satisfies 450mm≤L0≤650mm, the length of the battery cell is shorter, which helps to shorten the current diffusion path, reduce the internal resistance of the electrode, thereby reducing the heat generation of the battery and improving its dynamic performance. In addition, the shorter casing length helps to shorten the diffusion path of the electrolyte during the wetting process, improve the wetting rate and uniformity of the electrolyte, further promote the uniformity of lithium ion insertion and extraction during cycling, alleviate stress concentration, reduce the risk of film peeling, and improve the cycle stability of the battery cell.

[0051] In any embodiment, the length dimension L0 of the housing satisfies: 900mm≤L0≤1300mm.

[0052] When the length dimension L0 of the casing satisfies 900mm≤L0≤1300mm, the battery cell is relatively long, which helps to reduce the volume ratio of the casing in the battery cell and increase the load ratio of active materials. At the same time, a longer battery cell can reduce the number of batteries required in the battery module, simplify the structural design of the battery module, reduce the number and complexity of structural components in the module, thereby improving the space utilization of the battery pack and thus helping to improve the volumetric energy density of the battery cell.

[0053] In any embodiment, the material of the shell is a soft-pack material, which includes an aluminum-plastic composite film, and optionally includes one or more of aluminum, polypropylene (PP), polybutylene terephthalate (PBT), polybutylene succinate (PBS), nylon, polyethylene terephthalate (PET), and polyethylene (PE).

[0054] In any embodiment, the housing includes a first sealing area, which is disposed at at least one end of the laminated cell extending in the width direction; the first sealing area includes a folded edge structure extending in the length direction, on which encapsulating adhesive is disposed, and the encapsulating adhesive is continuously disposed in the length direction and fixes the folded edge structure.

[0055] In any embodiment, the housing includes at least one second sealing area, which is disposed at at least one end of the laminated cell along the length direction of the housing, and the second sealing area is disposed on the tab side of the laminated cell.

[0056] In any embodiment, the outer periphery of the laminated cell is provided with a plurality of rubber rings that surround in the width direction, and the rubber rings that surround in the width direction are spaced apart in the length direction.

[0057] The rubber rings that wrap around the width of the cell and are spaced apart along the length help to fix the position between the electrodes in the cell, reducing the probability of cell displacement during battery shaking. This is especially suitable for batteries with a large length, as it can effectively reduce the mutual displacement between the electrodes in the length direction, thus reducing lithium plating. This helps to maintain the stability of the internal spatial structure of the battery, thereby not affecting the normal operation of the battery.

[0058] In any embodiment, at 25°C, the capacity of the battery cell is 105Ah-190Ah, optionally 150Ah-190Ah.

[0059] A second aspect of this application provides a battery device including the battery cell described in the first aspect of this application.

[0060] A third aspect of this application provides an electrical device, which includes the battery device described in the second aspect of this application, the battery device being used to provide electrical energy.

[0061] A fourth aspect of this application provides an energy storage device, which includes the battery device described in the second aspect of this application, the battery device being used to store electrical energy. Attached Figure Description

[0062] Figure 1 is a schematic diagram of a diaphragm according to an embodiment of this application;

[0063] Figure 2 is a schematic diagram of a diaphragm in the prior art;

[0064] Figure 3 is a schematic diagram of the surface morphology of the adhesive layer according to an embodiment of this application;

[0065] Figure 4 is a schematic diagram of a pouch-pack stacked battery according to this application;

[0066] Figure 5 is a schematic diagram of an electrical device according to an embodiment of this application.

[0067] Explanation of reference numerals in the attached figures: 5. Battery cell; 50. Casing; 20. Separator; 201. Base film; 202. Ceramic layer; 203. Adhesive layer; X. Length direction; Y. Width direction; Z. Thickness direction. Detailed Implementation

[0068] The following detailed description, with appropriate reference to the accompanying drawings, discloses embodiments of the battery cell, battery device, power consumption device, and energy storage device of this application. However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repetitive descriptions of practically identical structures may be omitted. This is to avoid unnecessarily lengthy descriptions and to facilitate understanding by those skilled in the art. Furthermore, the accompanying drawings and the following description are provided for the purpose of enabling those skilled in the art to fully understand this application and are not intended to limit the subject matter of the claims.

[0069] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values ​​of 1 and 2 are listed, and if maximum range values ​​of 3, 4, and 5 are listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0070] Unless otherwise specified, all embodiments and optional embodiments of this application may be combined with each other to form new technical solutions, and such technical solutions should be considered to be included in the disclosure of this application.

[0071] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions, and such technical solutions shall be deemed to be included in the disclosure of this application.

[0072] Unless otherwise specified, all steps in this application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the method may also include step (c), indicating that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.

[0073] In this application, the terms "multiple" or "various" refer to two or more kinds.

[0074] Unless otherwise stated, the terms used in this application have the common meanings as commonly understood by those skilled in the art.

[0075] Unless otherwise stated, the values ​​of the parameters mentioned in this application can be determined using various testing methods commonly used in the art, for example, according to the testing methods given in the embodiments of this application. Unless otherwise stated, the test temperature for each parameter is 25°C.

[0076] In embodiments of this application, the battery device may include one or more battery cell assemblies for providing voltage and capacity. A battery cell assembly may include multiple pouch cell batteries connected in series, parallel, or a combination of these pouch cell batteries via a busbar. For example, a battery cell assembly is typically formed by arranging multiple pouch cell batteries; a battery cell assembly may also be a battery module, which is formed by arranging and fixing multiple pouch cell batteries into a single module. As an example, a battery module may be formed by bundling multiple battery cells together with cable ties.

[0077] The battery device can be a battery pack, which includes a housing and one or more individual battery cells housed within the housing. The individual battery cells can be battery modules, which can be housed within the housing by fixing the battery modules to the housing; alternatively, multiple pouch battery cells can be directly fixed to the housing and housed within the housing.

[0078] In embodiments of this application, the housing may include a first housing and a second housing. The first housing and the second housing are fastened together to form a closed space inside the housing for housing individual battery cells. Here, "closed" refers to covering or shutting down; it can be sealed or unsealed. The first housing may be a top cover or a bottom plate. For example, the housing may include a top cover, a frame, and a bottom plate. The top cover and the bottom plate are respectively connected to the frame, forming a closed space inside the housing for housing individual battery cells.

[0079] In embodiments of this application, the housing can be part of the vehicle's chassis structure. For example, a portion of the housing can be at least a part of the vehicle's floor, or a portion of the housing can be at least a part of the vehicle's crossbeams and longitudinal beams.

[0080] In this embodiment, the battery cell can be a rechargeable battery, which refers to a battery cell that can be recharged after discharge to activate the active materials and continue to be used; the battery cell can be a lithium-ion battery. The battery cell can be flat.

[0081] The battery mentioned in the embodiments of this application can be a single physical module comprising one or more battery cells to provide higher voltage and capacity. For example, the battery mentioned in this application can include battery cells, battery modules, or battery packs.

[0082] A single battery cell is the smallest unit that makes up a battery, and it can independently perform the functions of charging and discharging.

[0083] When there are multiple battery cells, they are connected in series, parallel, or mixed via a busbar. In some embodiments, the battery can be a battery module; when there are multiple battery cells, they are arranged and fixed to form a battery module. In some embodiments, the battery can be a battery pack, which includes a housing and battery cells, with the battery cells or battery modules housed within the housing. In some embodiments, the housing can be part of the vehicle's chassis structure. For example, a portion of the housing can be at least part of the vehicle's floor, or a portion of the housing can be at least part of the vehicle's crossbeams and longitudinal beams.

[0084] In some implementations, the battery can be an energy storage device. Energy storage devices include energy storage containers, energy storage cabinets, etc.

[0085] In some implementations, individual battery cells can be assembled into a battery module, and the number of individual battery cells contained in the battery module can be multiple, with the specific number adjustable according to the application and capacity of the battery module.

[0086] In some embodiments, the battery modules described above can also be assembled into a battery pack, and the number of battery modules contained in the battery pack can be adjusted according to the application and capacity of the battery pack.

[0087] A single battery cell includes electrode components and an electrolyte.

[0088] Electrode assemblies typically include positive and negative electrodes. The negative electrode is the electrode that absorbs or lithiates lithium ions during charging and releases or delithiates lithium during discharging. The positive electrode is the electrode that absorbs or delithiates lithium ions during charging and absorbs or lithiates lithium during discharging.

[0089] While lithium transition metal phosphate (LMT) particles offer significant advantages in cycle stability as positive electrode active materials, their intrinsic specific capacity is significantly lower than that of ternary materials. The applicant discovered that the capacity and energy density disadvantages can be compensated for by increasing the compaction density of LMT particles and combining it with a laminated cell structure. However, this process optimization also presents new technical challenges: compared to ternary materials, LMT particles are more structurally stable and less prone to breakage under high pressure. Therefore, LMT particles are often subjected to higher pressures during electrode compaction to achieve higher compaction density. Under high compaction density conditions, if the material's slippage ability is insufficient, stress concentration can easily occur during electrode rolling. Secondly, laminated cells, lacking the corners of wound cells, have a higher energy density compared to wound cells. However, the absence of corner constraints weakens the internal compressive force on the positive electrode membrane, making it easier for the positive electrode membrane to detach from the mold. Film shedding not only directly reduces the amount of active material participating in electrochemical reactions, but also leads to an "island" effect, where isolated regions form between particles or between particles and conductive agents, preventing proper electrical contact and thus hindering participation in the charge-discharge process, resulting in a sharp drop in battery capacity. Furthermore, the detached active material obstructs ion transport pathways, increases internal battery resistance, triggers localized overheating, and even increases the risk of thermal runaway, severely impacting battery cycle life and safety.

[0090] Based on this, the first aspect of this application provides a battery cell, including a stacked cell, the stacked cell including a positive electrode and a negative electrode, the positive electrode including a positive current collector and a positive electrode film layer disposed on at least one side of the positive current collector, the positive electrode film layer including lithium transition metal phosphate particles of carbon material disposed on at least a portion of its surface, and the median C of the graphitization degree C value of the positive electrode film layer obtained in the surface scanning mode of laser microscopy confocal Raman spectroscopy. 50 The value ranges from 0.95 to 1.20, where the degree of graphitization C is I. G / I D I G This indicates that the Raman spectrum is at 1580±100 cm⁻¹ - 1 The intensity of peak G at I D This indicates that the Raman spectrum is at 1350±100 cm⁻¹ -1 The D peak intensity at this point indicates that, with the battery cell in a fully discharged state, the compaction density of the positive electrode sheet is 2.3 g / cm³. 3 -2.6g / cm 3 .

[0091] The battery cell provided in this application improves the problem of capacity drop while having high capacity, and takes into account the cycle life of the battery.

[0092] Unconstrained by any theory, this may be because: adopting a stacked cell structure reduces the existence of ineffective space within the cell, effectively eliminating unavoidable corner gaps and interlayer gaps in the winding process, making the entire cell structure more compact, thereby improving space utilization, increasing the volumetric energy density of the battery cell, and increasing battery capacity; in addition, the regularity of the stacked structure also creates favorable conditions for improving the high compaction density process of the electrodes. Within the same volume, a stacked cell can accommodate more electrode sheets, and with high compaction density electrodes, further improves the battery's energy density and capacity output. Meanwhile, the applicant obtained the median C of the graphitization degree C value in the cumulative distribution curve of the positive electrode film layer under laser microscopy confocal Raman spectroscopy scanning mode. 50 To achieve a balance between battery capacity and cycle performance. The median C of graphitization degree of the positive electrode film obtained in laser microscopy confocal Raman spectroscopy instrument scanning mode. 50 This reflects the degree of graphitization of the carbon coating material on the surface of lithium transition metal phosphate (LiMT) particles, i.e., the degree of orderliness of the carbon coating material on the surface of LiMT particles. A higher degree of graphitization in LiMT particles indicates a more ordered arrangement of carbon atoms, forming a near-ideal graphitic layered structure. This structure effectively reduces interparticle friction, facilitating relative sliding along the interlayer under stress, exhibiting good slippage capability. This helps alleviate stress concentration in the film layer, reduces the risk of film delamination, and ultimately improves the cycle life of the battery.

[0093] In this application, a laminated cell refers to a cell formed by stacking a positive electrode, a separator, and a negative electrode together.

[0094] In this application, the positive electrode film layer contains lithium transition metal phosphate particles. However, the positive electrode film layer does not refer solely to the positive electrode active material layer. Other film layers that are connected to the positive electrode active material layer and are difficult to distinguish, such as the undercoat layer and the liquid retention layer, are collectively referred to as the positive electrode film layer.

[0095] In this application, lithium-containing transition metal phosphate particles refer to phosphate materials containing lithium and transition metal elements, which can be detected by any method known in the art. For example, they can be detected by combining X-ray diffraction (XRD) with energy dispersive spectroscopy (EDS) or inductively coupled plasma mass spectrometry (ICP-MS).

[0096] In this application, the carbon coating material disposed on at least a portion of the surface of lithium-containing transition metal phosphate particles can be detected by any method known in the art. As an example, the carbon coating material disposed on at least a portion of the surface of lithium-containing transition metal phosphate particles can be observed by characterizing the particles using a combination of transmission electron microscopy and energy dispersive spectroscopy.

[0097] In this application, the fully discharged state refers to the state after the battery is placed in a 25°C oven environment, left to stand for 2 hours, and the battery temperature is maintained at 25°C, and then discharged at a constant current of 1 / 3C to 2.5V and then discharged at a constant current of 0.1C to 2.0V.

[0098] The compaction density of the positive electrode sheet can be tested using methods known in the art. As an example, the battery is placed in a 25°C oven environment and left to stand for 2 hours. After the battery temperature is maintained at 25°C, the battery is discharged at a constant current of 1 / 3C to 2.5V and then discharged at a constant current of 0.1C to 2.0V. The battery is then disassembled to obtain the positive electrode sheet. The residual electrolyte is treated with dimethyl carbonate solvent, the electrode sheet is dried, and it is cut into small circular pieces with an area of ​​S. The mass of the circular pieces is obtained as W1, and the thickness of the positive electrode sheet is measured using a micrometer. Then, the positive electrode film layer of the weighed electrode sheet is wiped off, the mass of the current collector is weighed and recorded as W2, and the thickness of the current collector is measured using a micrometer. Then, the compaction density of the positive electrode sheet is PD=(W1-W2) / [(T1-T2)×S].

[0099] In some embodiments, the compaction density of the positive electrode sheet of the battery cell in its fully discharged state can be selected as 2.3 g / cm³. 3 2.31 g / cm 3 2.32 g / cm 3 2.33 g / cm 3 2.34 g / cm 3 2.35g / cm 3 2.36 g / cm 3 2.37 g / cm 3 2.38g / cm 3 2.39 g / cm 3 2.40 g / cm 3 2.41 g / cm 3 2.42 g / cm 3 2.43 g / cm 3 2.44 g / cm 3 2.45g / cm 3 2.46 g / cm 3 2.47 g / cm 3 2.48 g / cm 3 2.49 g / cm 3 2.50g / cm 3 2.55g / cm 3 2.60g / cm 3 Or the range of values ​​between any two.

[0100] In this application, the cumulative distribution curve of graphitization degree C value refers to the curve obtained by arranging at least 100 C values ​​in ascending order, with graphitization degree as the horizontal axis and the cumulative percentage as the vertical axis. 50 This represents the C value corresponding to a cumulative percentage of 50% on the vertical axis of the cumulative distribution curve of graphitization degree C. The median C value of graphitization degree. 50 Compared to point values, it can reflect the overall graphitization degree of particles in the positive electrode film, i.e., the degree of slippage; compared to the mean value, it can reduce the influence of extreme values ​​during the test and improve the confidence of the test results.

[0101] The graphitization degree (C-value) of the positive electrode film can be obtained using a laser confocal Raman spectroscopy (LCS) surface scanning mode. Specifically, a high-precision Renishaw laser confocal Raman spectroscopy system (LCS) is used, with an excitation wavelength of 532 nm. A suitable amount of the positive electrode film is scanned on its surface or along a section of the electrode thickness. The scanning area is 45 μm × 45 μm, divided into 10 × 10 grids, with grid vertices as test points, a step size of 5 μm, and a total of 100 scan points. This yields the C-values ​​at different sites and the cumulative distribution curve of the C-values ​​in the scanned area. The positive electrode film in this application can be either freshly prepared or obtained from dismantling a battery. Positive electrode films obtained from dismantling batteries inevitably have residual electrolyte salt particles on their surface. To improve testing accuracy, it is preferable to perform a surface scan on a section of the positive electrode film along the electrode thickness direction to characterize the graphitization degree of the positive electrode film.

[0102] The graphitization degree C of the positive electrode film was obtained by the ratio of the peak intensities of the G-band and D-band in the Raman spectrum. The position of the G-band peak was 1580±100 cm⁻¹. -1 Its characterization of carbon sp 2 Hybrid structure; D peak position is 1350±100 cm⁻¹ -1 It characterizes a disordered structure, where disorder refers to the irregular arrangement of carbon atoms within the structure. In graphite crystals, carbon atoms in the same layer arrange themselves in an sp... 2 Hybridization forms covalent bonds, while interlayer bonding is facilitated by van der Waals forces, making the carbon in the graphite structure prone to slip. Therefore, the C value can characterize the degree of graphitization in the cathode film. It is understandable that the degree of graphitization in the cathode film mainly originates from the graphitized carbon material within the film, i.e., the carbon coating material of the cathode active material. Although rich in sp... 2 Hybridized carbon nanotube conductive agents also have relatively high I0 G / I D However, due to its low content and small tube diameter, its addition to the positive electrode film results in an extreme value in the Raman surface scan test of the positive electrode film, and does not affect the graphitization degree C in the positive electrode film.50 This has an impact. Therefore, the degree of graphitization of the positive electrode film can also be used to characterize the degree of graphitization of the positive electrode active material.

[0103] Those skilled in the art can control the degree of graphitization of active material particles using any known process. For example, adjusting the carbon source, sintering temperature, sintering time, sintering pressure, and sintering atmosphere can all achieve adjustments to the degree of graphitization of active material particles.

[0104] The higher the degree of graphitization of carbon on the surface of the positive electrode active material, the higher the proportion of graphite structure carbon in the positive electrode film layer. The particles are more likely to slip by means of the highly graphitized carbon structure in the coating layer, which reduces stress concentration in the electrode, reduces demolding, and improves the cycle performance of the battery.

[0105] In some embodiments, the median C of the graphitization degree C in the cumulative distribution curve of the positive electrode film obtained in the laser microscopy confocal Raman spectroscopy instrument scanning mode is... 50 The value can be selected from 0.95, 0.96, 0.97, 0.98, 0.99, 1.00, 1.01, 1.02, 1.03, 1.04, 1.05, 1.06, 1.07, 1.08, 1.09, 1.10, 1.11, 1.12, 1.13, 1.14, 1.15, 1.16, 1.17, 1.18, 1.19, 1.20, or any value range between the two.

[0106] In some embodiments, the median C of the graphitization degree C in the cumulative distribution curve of the positive electrode film obtained in the laser microscopy confocal Raman spectroscopy instrument scanning mode is... 50 The value is 1.01-1.13.

[0107] If the graphitization degree of the positive electrode film is further within the above range, it will help to further improve the slippage of particles in the positive electrode film, reduce stress concentration in the positive electrode film, and thus further improve the long-cycle stability of the battery cell.

[0108] In some embodiments, the concentration of C values ​​(C0.05) in the cumulative distribution curve of graphitization degree C values ​​obtained by laser microscopy confocal Raman spectroscopy in instrument scanning mode is... 90 -C 10 ) / C 50 It ranges from 0.01 to 0.05.

[0109] Referring to the above, and by analogy, C 90 C represents the C value corresponding to a cumulative percentage of 90% on the vertical axis of the cumulative distribution curve of graphitization degree C. 10This represents the C-value on the vertical axis of the cumulative distribution curve of graphitization degree C, corresponding to a cumulative percentage of 10%. The concentration of C-values ​​is expressed as (C... 90 -C 10 ) / C 50 Indicates. (C) 90 -C 10 ) / C 50 It can reflect the magnitude of most C values, is unaffected by extreme values, and also reflects the width of the graphitization distribution of particles in the cathode film. A low concentration of C values ​​in the cathode film indicates a narrow width and good concentration of the graphitization distribution of particles in the cathode film.

[0110] In some embodiments, the concentration of C values ​​(C0) in the cumulative distribution curve of graphitization degree C values ​​obtained by laser microscopy confocal Raman spectroscopy in instrument scanning mode is... 90 -C 10 ) / C 50 The value can be selected as 0.01, 0.02, 0.023, 0.025, 0.03, 0.035, 0.036, 0.039, 0.04, 0.045, 0.05, or any value range between the two.

[0111] The concentration of C value in the positive electrode film is 0.01-0.05, which indicates that the graphitization degree of the particles in the positive electrode film is highly consistent. This means that the positive electrode active material has good coating uniformity and consistency, which can reduce the slip resistance caused by the inconsistency of the graphitization degree of the particles in the positive electrode active material and the resulting local stress concentration, reduce the risk of demolding, and thus improve the long-cycle stability of the battery cell.

[0112] In some embodiments, the concentration of C values ​​(C0.05) in the cumulative distribution curve of graphitization degree C values ​​obtained by laser microscopy confocal Raman spectroscopy in instrument scanning mode is... 90 -C 10 ) / C 50 It ranges from 0.02 to 0.04.

[0113] The median C of the graphitization degree of the positive electrode film 50 Within the aforementioned range, it is beneficial to further improve the slippage between particles, while maintaining the high dynamic performance of the battery and further reducing local stress concentration, reducing the risk of demolding, and achieving a balance between battery performance and energy density.

[0114] In some implementations, based on the total area of ​​particles in the cross section of the positive electrode film along the thickness direction of the electrode, the area ratio of particles with a particle size R1 satisfying R1≥1000nm is 12%-50%.

[0115] In this application, the term "particle" refers to a particle in the positive electrode film layer that has a identifiable complete boundary in the field of view at a certain magnification, such as 10,000x. Defects and scratches may exist inside the particle, but a complete boundary sufficient to divide the particle cannot be identified within it. The positive electrode film layer in this application can be a freshly prepared positive electrode film layer or a positive electrode film layer obtained from disassembly of a battery.

[0116] The particle identification method is as follows: The positive electrode film layer is cut along the thickness direction of the electrode sheet using an argon ion beam (for example, a Leica EMTIC3XCP device can be used, operating voltage: 6kV, operating time: 6h). After exposing the cut surface, a scanning electron microscope (SEM) is used (for example, a Hitachi SU8230 device can be used, operating voltage: 3kV, beam current: high, probe model: U (LA100), working distance <5mm) to observe the cut surface along the thickness direction of the electrode sheet. Images are acquired using a field emission scanning electron microscope at a non-edge location in the cut surface of the positive electrode film layer (after observing the electrode edge under the SEM, the field of view is adjusted to the center of the sample) in secondary electron mode. Electron micrographs are taken at 10kx magnification, and the particles in the electron micrographs are analyzed using ImageJ software (1.46r, win64 version). The specific steps for using ImageJ software are as follows: Load the scanning electron microscope (SEM) image to be analyzed; use the Cellpose plugin to identify particles, and then perform manual corrections; use ImageJ to read and analyze data. The specific method for using the Cellpose plugin to identify particles is as follows: Set the segmentation diameter parameter (diameter in the Segmentation module) to 15 pixels, click "runcyto3" to identify particles; manually mark particles in the image that were not identified by the software, were not fully identified, or were identified incorrectly. Particles that were not identified by the software, were not fully identified, or were identified incorrectly mainly include the following: 1. Particles that are too large or have scratches on their surface, making them unidentifiable or incompletely identifiable; 2. During argon ion beam cutting, scratches may be generated on the particle surface, and the software may misinterpret these scratches as particle boundaries, leading to identification errors; 3. Particles that are too small and were not successfully identified; 4. Particles located at the edge of the SEM field of view, with the interior penetrated by the edge, preventing a complete view of the morphology, resulting in identification errors due to partial identification replacing the whole.For the unidentified or misidentified particles mentioned above, manual calibration is performed. The specific process is as follows: 1. Delete large particles located around the edges of the scanning electron microscope that are not fully displayed. 2. Determine if any unidentified or misidentified particles have internal cracks or scratches. If no cracks or scratches are found, classify it as a single particle and manually mark it based on the observed particle boundary. 3. If cracks or scratches are found inside the particle, determine if they penetrate the particle. If not, classify it as a single particle and manually mark it. 4. If cracks or scratches penetrate the particle, determine if they are linear or irregular. 5. If the cracks or scratches are irregular, classify them as the boundary between particles and divide the particles along this boundary. 6. If the cracks or scratches are linear, perform contrast comparison. 7. If the contrast is not obvious and there is no crack-like appearance, classify it as a scratch and mark it as a single particle. 8. If the contrast is strong and there is a crack-like appearance, classify it as the boundary between particles and mark it as two particles. After manual marking, delete information irrelevant to the particles from the automatic image processing, thus completing the particle identification and marking in the image.

[0117] It is understandable that the particles in the cross-section of the positive electrode film along the thickness direction, especially those larger than 50 nm, mainly originate from the positive electrode active material. Therefore, the embodiments of this application can accurately and objectively reflect the distribution of lithium transition metal phosphate particles in the positive electrode film by observing and statistically analyzing the particle area in the cross-section of the positive electrode along the thickness direction.

[0118] In existing technologies, laser particle size analyzers are typically used to statistically analyze the particle size of positive electrode active materials using Malvern laser diffraction. However, the applicant's research indicates that because lithium-containing transition metal phosphate particles are prone to agglomeration, the test results obtained by Malvern laser diffraction based on the principle of laser scattering often only reflect the particle size of the agglomerates, and cannot accurately reflect the particle size of the positive electrode active material, let alone its dispersion state in the film layer. This is because the dispersion of the positive electrode active material in the film layer increases during slurry preparation and film forming rolling. The test results obtained by Malvern laser diffraction are affected by the particle size, specific surface area, and degree of agglomeration of the positive electrode active material. Compared to the actual dispersion in the electrode sheet, the number of large particles obtained by this test is lower than the actual value, and the number of small particles is higher than the actual value. Therefore, the particle size obtained by Malvern laser diffraction cannot be equated with or analogized to the particle size statistically obtained in the embodiments of this application.

[0119] The method for testing the area ratio of particles with a diameter R1 satisfying R1≥1000nm in the cross-section of the positive electrode film along the electrode thickness direction is as follows: Particles in the positive electrode film are identified using the method described above in this application. The images after particle identification and labeling are imported into ImageJ software for analysis. A scale is set based on the scanning electron microscope image. The particle diameter, area, sphericity, and roughness in the cross-section of the positive electrode film along the electrode thickness direction are statistically analyzed using the "Feret diameter," "Area," "Round," and "Solidity" analysis functions. According to the software manual (ImageJ User Guide IJ 1.46r), the obtained "Feret" parameter represents the maximum spacing between all parallel lines in the two-dimensional projection of the particle, thus characterizing the particle diameter; the obtained "Area" parameter represents the pixel area of ​​the particle. Because particles smaller than 50nm are prone to significant errors during statistical analysis and are difficult to accurately identify, and because the particle size of conductive agents is generally smaller than 50nm, which can also introduce large errors into the statistical results, particles smaller than 50nm are not counted in the particle size statistics of this application, and the statistical data of particles whose AR, Round, or Solidity is displayed as "NaN" are deleted. The sum of the "Area" parameters of particles with a particle size R1 satisfying R1≥1000nm and the sum of the "Area" parameters of all particles are calculated, and these are respectively used as the area of ​​particles with a particle size R1 satisfying R1≥1000nm and the total area of ​​the counted particles. The sum of the areas of particles with a particle size R1 satisfying R1≥1000nm divided by the total area of ​​the counted particles is used as the proportion of the area of ​​particles with a particle size R1 satisfying R1≥1000nm in the cross-section of the positive electrode film along the thickness direction of the electrode sheet.

[0120] In some implementations, based on the total area of ​​particles in the cross-section of the positive electrode film along the thickness direction of the electrode sheet, the area percentage of particles with a particle size R1 satisfying R1≥1000nm can be selected as 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39%, 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49%, 50%, or any value range between the two.

[0121] In some implementations, based on the total area of ​​particles in the cross section of the positive electrode film along the electrode thickness direction, the area ratio of particles with a particle size R1 satisfying R1≥1000nm is 12%-40%.

[0122] Large particles with a particle size R1 ≥ 1000 nm help improve the compaction density of the positive electrode, thereby increasing the volumetric energy density of the battery cell. However, researchers have found that these large particles are prone to stress concentration, increasing the risk of positive electrode film delamination. Therefore, the area ratio of particles with a particle size R1 ≥ 1000 nm in the cross-section of the positive electrode film along the thickness direction should be in the range of 12%-50%, and further in the range of 12%-40%. This can improve the compaction density of the electrode without making the film delamination probability too high. This improves the energy density of thick-coated lithium transition metal phosphate batteries while alleviating the capacity drop problem and taking into account the cycle life of the battery.

[0123] In some embodiments, in the cumulative area distribution curve of spheroidal area for particles with a particle size R1 satisfying R1≥1000nm, L R1A50 It is 0.6-0.8.

[0124] In this application, the method for testing the sphericity of particles with a diameter R1 satisfying R1≥1000nm in a cross-section along the thickness direction of the positive electrode film is as follows: Particles in the cross-section of the positive electrode film are identified using the method described above. The morphology of the particles in the cross-section along the thickness direction of the electrode film is analyzed using the "Shape Description" analysis function in ImageJ. According to the software manual (ImageJ User Guide IJ 1.46r), the "Round" parameter obtained from the analysis represents the ratio of the pixel area of ​​the particle to the area of ​​a circle with the fitted major axis as its diameter, which can be used to characterize the sphericity of the particle. The closer the particle is to a sphere, the closer the ratio of the pixel area to the area of ​​the circle with the fitted major axis as its diameter is to 1. Therefore, the "Round" parameter of the particle obtained from the analysis is used to characterize the sphericity of the particle. Following the above method, to ensure a statistically significant sample size, at least 10 non-overlapping scanning electron microscope images are acquired for each electrode. The sphericity of at least 1000 particles was arranged in ascending order, and the cumulative sphericity distribution curve of the particles in the positive electrode film was obtained with sphericity as the horizontal axis and cumulative area ratio as the vertical axis. L A50 This is the L-value of sphericity that corresponds to the cumulative area ratio of the vertical axis in the cumulative distribution curve of granular sphericity L-values ​​being 50%.

[0125] In some embodiments, in the cross-section of the positive electrode film along the thickness direction of the positive electrode sheet, in the cumulative distribution curve of the spheroidal area of ​​particles with a particle size R1 satisfying R1≥1000nm, L R1A50The value can be selected from 0.60, 0.61, 0.62, 0.63, 0.64, 0.65, 0.66, 0.67, 0.68, 0.69, 0.70, 0.705, 0.71, 0.72, 0.73, 0.74, 0.75, 0.76, 0.77, 0.78, 0.79, 0.80, or any value range between the two.

[0126] Those skilled in the art can control the sphericity of particles using any known process. For example, the sphericity of particles can be adjusted through processes such as grinding, polishing, chemical etching, mechanical stirring, extrusion, coating, granulation, and adding surfactants, as well as by adjusting the parameters of each process.

[0127] In some embodiments, in the cross-section of the positive electrode film along the thickness direction of the positive electrode sheet, in the cumulative distribution curve of the spheroidal area of ​​particles with a particle size R1 satisfying R1≥1000nm, L R1A50 It is 0.65-0.75.

[0128] In some embodiments, in the cross-section of the positive electrode film along the thickness direction of the positive electrode sheet, in the cumulative distribution curve of the spheroidal area of ​​particles with a particle size R1 satisfying R1≥1000nm, L R1A50 It is 0.67-0.75.

[0129] In the cross-section of the positive electrode film along the thickness direction of the positive electrode sheet, in the cumulative area distribution curve of the spheroidal area of ​​particles with a particle size R1 satisfying R1≥1000nm, L R1A50 Within the range of 0.65-0.75, and further within the range of 0.67-0.75, it is beneficial to further reduce the stress concentration at large particles in the positive electrode film layer of the thick-coated laminated cell, thereby reducing the probability of film layer peeling and improving the cycle life of the battery.

[0130] In some implementations, the median B of the coating value B in the cumulative distribution curve of the positive electrode film obtained in laser microscopy confocal Raman spectroscopy instrument scanning mode is... 50 The value is 0.30-0.60, where the coating value B is I. P / I D , where I P This indicates that the Raman spectrum is at 948±100 cm⁻¹ -1 The intensity of the P peak at I D This indicates that the Raman spectrum is at 1350±100 cm⁻¹ -1 The intensity of peak D at that location.

[0131] The cumulative distribution curve of the coating value (B-value) is obtained by arranging at least 100 B-values ​​in ascending order, with the coating value on the horizontal axis and the cumulative percentage on the vertical axis. To reduce the influence of extreme coating values ​​caused by non-particle regions in the positive electrode film on the test results, the median coating value (B-value) is used. 50 Evaluate the density of the carbon coating material on the positive electrode active material. (B) 50 The B value is the value corresponding to the cumulative number of values ​​on the vertical axis of the cumulative distribution curve of the coverage value B value when the cumulative number accounts for 50%.

[0132] In this application, the coating value (B-value) of the positive electrode film can be obtained by scanning with a laser confocal microscopy (LCM) spectrometer. Specifically, a high-precision Renishaw laser confocal microscopy (LCM) spectrometer is used, with an excitation wavelength of 532 nm. A suitable amount of the positive electrode film is scanned on its surface or along a section of the electrode thickness. The scanning area is 45 μm × 45 μm, divided into 10 × 10 grids, with grid vertices as test points, a step size of 5 μm, and a total of 100 scan points. This yields the B-values ​​at different locations and the cumulative distribution curve of the B-values ​​in the scanned area. The positive electrode film in this application can be either freshly prepared or obtained from disassembly from a battery. Positive electrode films obtained from disassembly inevitably have residual electrolyte salt particles on their surface. To improve testing accuracy, it is preferable to perform a surface scan on a section of the positive electrode film along the electrode thickness to characterize the coating value.

[0133] The coating value B of the positive electrode film was obtained by the ratio of the peak intensities of the P-band and D-band in the Raman spectrum, with the P-band located at 948±100 cm⁻¹. -1 Its characterization of phosphate PO4 3- Structure; D peak position is 1350±100cm -1 The characterization of the structure is based on disorder, where disorder refers to the irregular arrangement of carbon atoms within the structure. During the testing process, an excitation wavelength of 532 nm was selected, resulting in a shallow testing depth. Consequently, in the test results obtained using laser microscopy confocal Raman spectroscopy in surface scanning mode, the carbon structure peak exhibited a higher intensity compared to the phosphate structure peak.

[0134] Those skilled in the art can control the coating value of active material particles using any known process. For example, adjusting the carbon source type, carbon source addition amount, sintering temperature, sintering time, sintering pressure, and sintering atmosphere can all achieve adjustments to the coating value of the active material particles. The coating value (B-value) reflects the density of the carbon coating material on the surface of lithium transition metal phosphate particles. The denser the carbon coating, the lower the relative intensity of the phosphate structure detected in the Raman spectrum, and the smaller the coating value (B-value) of the positive electrode film.

[0135] In some embodiments, the positive electrode film further includes a coating layer disposed on at least a portion of the surface of the lithium-containing transition metal phosphate particles, wherein the median B of the coating value B in the cumulative distribution curve of the positive electrode film obtained in laser microscopy confocal Raman spectroscopy instrument scanning mode is... 50 The value can be selected from 0.3, 0.31, 0.32, 0.33, 0.34, 0.35, 0.36, 0.37, 0.38, 0.39, 0.4, 0.41, 0.42, 0.43, 0.44, 0.45, 0.46, 0.47, 0.48, 0.49, 0.5, 0.51, 0.52, 0.53, 0.54, 0.55, 0.56, 0.57, 0.58, 0.59, 0.6, or any value range between the two.

[0136] The median B of the coating value of the positive electrode film 50 Within the aforementioned range, it is evident that the carbon coating material of the positive electrode active material is relatively dense and uniform, which is beneficial for improving the slip uniformity of the positive electrode film during the rolling process and reducing stress concentration in the thick-coated positive electrode film. In addition, thanks to the dense and uniform carbon coating material, large particles in the positive electrode film are more likely to slip during the compaction process, thereby reducing stress concentration at large particles in the thick-coated positive electrode film, reducing the probability of positive electrode film detachment, improving the problem of battery capacity drop, and increasing the cycle life of the battery.

[0137] In some implementations, the thickness H of the positive electrode film on one side is 70 μm-120 μm.

[0138] In some embodiments, the thickness H of the positive electrode film on one side is 90 μm-120 μm.

[0139] The thickness of the positive electrode film can be measured using any method known in the art. As an example, the thickness of the positive electrode film in a cross-section along the thickness direction of the positive electrode sheet is measured using a scanning electron microscope.

[0140] In some embodiments, the single-sided thickness H of the positive electrode film can be selected as 70 μm, 71 μm, 71.53 μm, 72 μm, 73 μm, 74 μm, 75 μm, 76 μm, 77 μm, 78 μm, 79 μm, 80 μm, 81 μm, 82 μm, 83 μm, 84 μm, 85 μm, 86 μm, 87 μm, 88 μm, 89 μm, 90 μm, 91 μm, 92 μm, 93 μm, 94 μm, 95 μm, 96 μm, 97 μm, 98 μm, 99 μm, 1 00μm, 101μm, 102μm, 103μm, 104μm, 105μm, 105.64μm, 105.89μm, 106μm, 106.66μm, 106.79μm, 107μm, 108μm, 109μm, 110μm, 111μm, 112μm, 113μm, 114μm, 115μm, 116μm, 117μm, 118μm, 119μm, 119.12μm, 120μm or any range between the two.

[0141] During long-term battery cycling, excessive thickness of the positive electrode film can lead to significant volume expansion, increasing internal stress and making the electrode more susceptible to film detachment in the later stages of cycling. Maintaining a single-sided thickness within the aforementioned range helps to further increase the loading of positive electrode active materials in the battery, thereby improving battery capacity, while simultaneously reducing the risk of film detachment and enhancing battery cycle performance.

[0142] In some embodiments, the thickness H of the positive electrode film on one side is 100 μm-120 μm.

[0143] Increasing the thickness of the positive electrode film helps to increase the loading of the positive electrode active material and thus improves the battery capacity. However, the applicant has found that when the single-sided thickness of the positive electrode film is greater than or equal to 100 μm, the volume expansion of the positive electrode film is more significant during battery cycling, resulting in greater stress. This leads to more pronounced stress concentration in the positive electrode film, increasing the risk of film detachment and consequently affecting the battery's cycle performance. The embodiments of this application increase the battery capacity by increasing the thickness of the positive electrode film, while simultaneously controlling the median C of the graphitization degree C value in the cumulative distribution curve obtained under laser microscopy confocal Raman spectroscopy surface scanning mode. 50 This improves the slippage ability between particles in the positive electrode film, thereby helping to reduce stress concentration in the film, reducing the risk of film shedding, and thus improving the cycle life of the battery.

[0144] In some embodiments, the lithium transition metal phosphate particles in the positive electrode film layer comprise components represented by the following general formula: Li m Fe x P y Oj Q q Formula I,

[0145] Wherein, Q includes one or more of Al, Na, K, Mg, Cu, Mn, Cr, Zn, Pb, Ca, Co, Ni, Sr, Nb, V, Ti, B, S, Si, N, F, Cl, and Br, with 0.8≤m≤1.15, 0.9≤x≤1, 0.95≤y≤1, 3.5≤j≤4, and 0≤q≤0.1.

[0146] In some implementations, m can be selected as 0.8, 0.85, 0.9, 0.95, 0.98, 1.00, 1.03, 1.05, 1.08, 1.10, 1.13, 1.15, or any value range between two of these; x can be selected as 0.9, 0.91, 0.92, 0.93, 0.94, 0.95, 0.96, 0.97, 0.98, 0.99, 1.0, or any value range between two of these. y can be 0.95, 0.96, 0.97, 0.98, 0.99, 1.00 or any value between two of these; j can be 3.5, 3.6, 3.7, 3.8, 3.9, 4 or any value between two of these; q can be 0, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1 or any value between two of these.

[0147] In some embodiments, the lithium-containing transition metal phosphate particles in the positive electrode film include one or more of lithium iron phosphate, lithium manganese phosphate, lithium fluorinated vanadium phosphate, lithium manganese iron phosphate, and their modified materials.

[0148] In some embodiments, the lithium-containing transition metal phosphate particles in the positive electrode film include one or more of lithium iron phosphate and its doped and modified materials, and coating and modified materials.

[0149] In some implementations, the iron leaching rate of the cathode material is 658ppm-1921ppm.

[0150] The iron dissolution rate of the cathode material can be tested using methods known in the art. As an example, 7.5g of cathode material powder obtained by scraping from the cathode film sample is weighed and added to 100.3g of 0.3% ascorbic acid solution (solvent is ultrapure water). After stirring at 500 rpm for 305 minutes, the solution is quickly aspirated using a 5mL syringe and filtered into a test tube using a 0.45μm pore size filter. 1mL of the supernatant is aspirated using a pipette and added to a glass volumetric flask for 50-fold dilution. The iron concentration in the solution is obtained by inductively coupled plasma mass spectrometry (ICP-OES). The iron dissolution rate of the cathode material is calculated using the formula: (ICP test iron concentration × solution volume / mass of the solution used for volume adjustment) × 100.3g / mass of cathode material powder, where the solution volume is 50mL and the mass of the solution used for volume adjustment is 1g.

[0151] In some embodiments, the iron dissolution rate of the cathode material can be 658ppm, 700ppm, 800ppm, 890ppm, 900ppm, 1000ppm, 1058ppm, 1076ppm, 1100ppm, 1143pm, 1200ppm, 1236pm, 1300ppm, 1311pm, 1384pm, 1349pm, 1400ppm, 1485pm, 1500ppm, 1531pm, 1600ppm, 1700ppm, 1800ppm, 1921ppm, or any value between the two.

[0152] In some implementations, the iron leaching rate of the cathode material is 658ppm-1485ppm.

[0153] The iron dissolved in the cathode material mainly originates from lithium transition metal phosphate particles in the cathode active material. The iron dissolution rate depends on the number of lattice defects in the lithium transition metal phosphate and the integrity and density of the carbon coating on the surface of the cathode active material. A lower iron dissolution rate means fewer lattice defects in the lithium transition metal phosphate, which helps reduce lattice corrosion in weak acid environments. Furthermore, a more complete and dense carbon coating on the surface of the cathode active material inhibits the dissolution of iron ions in weak acid environments. Cathode materials with iron dissolution rates within the above range have relatively few lattice defects and complete, dense carbon coatings, which helps improve the compressive strength and slippage of particles in the cathode film under high rolling pressure, increases the compaction density of the cathode film, reduces stress concentration in the cathode film, improves the energy density of the battery, and also addresses the issue of battery capacity drops.

[0154] In some implementations, the mass content of titanium is 500ppm-8000ppm based on the total mass of lithium transition metal phosphate particles in the positive electrode film.

[0155] The types and contents of elements in lithium transition metal phosphate particles in the positive electrode film can be tested using any method known in the art. As an example, inductively coupled plasma atomic emission spectrometry (ICP-AES) was used to test the titanium content, referring to Appendix C of GB / T 33822-2017.

[0156] In some embodiments, based on the total mass of lithium transition metal phosphate particles in the positive electrode film, the mass content of titanium can be selected as 500ppm, 600ppm, 700ppm, 800ppm, 900ppm, 1000ppm, 1100ppm, 1200ppm, 1400ppm, 1500ppm, 1600ppm, 1700ppm, 1800ppm, 1900ppm, 2000ppm, 2100ppm, 2200ppm, 2300ppm, 2400ppm, 2500ppm, 2600ppm, 2700ppm, 2800ppm, 2900ppm, 3000ppm, 3500ppm, 4000ppm, 4500ppm, 5000ppm, 5500ppm, 6000ppm, 6500ppm, 7000ppm, 7500ppm, 8000ppm, or any value range between the two.

[0157] In some embodiments, the mass content of titanium is 1000ppm-3000ppm based on the total mass of lithium transition metal phosphate particles in the positive electrode film.

[0158] Introducing titanium into lithium transition metal phosphate particles requires adding a titanium source during the preparation of the cathode active material. Titanium sources are often inert materials, and their adhesion to the surface of the lithium transition metal phosphate particles reduces reactivity and particle size growth. Increasing the graphitization degree of the cathode active material often requires higher sintering temperatures or longer sintering times, but this also increases the particle size in the cathode film, increasing stress concentration and potentially causing film detachment. In this embodiment, by adding a high content of titanium to the lithium transition metal phosphate particles, the reactivity of the cathode active material synthesis raw materials is reduced. This allows the cathode active material to achieve high graphitization while controlling the proportion of large particles, reducing stress concentration in the cathode film, lowering the probability of film detachment, and improving both battery energy density and cycle life.

[0159] Meanwhile, the doping of titanium in the positive electrode active material is beneficial for inducing lattice distortion, reducing Li-O bond energy, increasing lithium-ion transport rate, and improving the kinetic performance of the battery. In thick coated films, lithium-ion diffusion is uneven, often accompanied by a significant lithium-ion concentration gradient. This application's embodiments improve the solid-phase transport rate of the positive electrode active material by adding a high content of titanium to lithium-containing transition metal phosphate particles, thus addressing the kinetic problems of thick electrode batteries.

[0160] In some implementations, the vanadium content is 500 ppm to 5000 ppm based on the total mass of lithium transition metal phosphate particles in the positive electrode film.

[0161] The types and contents of elements in lithium transition metal phosphate particles in the positive electrode film can be tested using any method known in the art. As an example, inductively coupled plasma atomic emission spectrometry (ICP-AES) is used to test the vanadium content, referring to Appendix C of GB / T 33822-2017.

[0162] In some embodiments, the vanadium content can be selected as 500ppm, 600ppm, 700ppm, 800ppm, 900ppm, 1000ppm, 1100ppm, 1200ppm, 1400ppm, 1500ppm, 1600ppm, 1700ppm, 1800ppm, 1900ppm, 2000ppm, 2100ppm, 2200ppm, 2300ppm, 2400ppm, 2500ppm, 2600ppm, 2700ppm, 2800ppm, 2900ppm, 3000ppm, 3500ppm, 4000ppm, 4500ppm, or 5000ppm, based on the total mass of lithium transition metal phosphate particles in the positive electrode film.

[0163] In some implementations, the vanadium content is 500 ppm to 3000 ppm based on the total mass of lithium transition metal phosphate particles in the positive electrode film.

[0164] Vanadium in the positive electrode film can exist in multiple valence states. Vanadium in the +5 valence state (V5+) can be doped into phosphorus sites. Due to its large radius, it can cause lattice distortion, expanding the diffusion channels for lithium ions, thereby improving the ionic conductivity of the positive electrode active material and enhancing the battery's kinetic performance. Vanadium in the +3 valence state (V... 3+ Vanadium can be doped into transition metal sites, generating lithium vacancies through charge compensation, thereby improving the electronic conductivity of the positive electrode active material. Furthermore, the increased uniformity of vanadium distribution in lithium-containing transition metal phosphate particles helps to further improve the kinetic performance and reaction uniformity of the positive electrode film, thus further enhancing the kinetic and cycle performance of the battery cell.

[0165] Vanadium content within the aforementioned range helps improve the kinetic performance of the positive electrode and the kinetic performance of thick-coated lithium transition metal phosphate batteries. Simultaneously, the synergistic effect of titanium, vanadium, and carbon nanotubes in the positive electrode film helps form a good three-dimensional network, further improving the electronic and ionic conductivity of the positive electrode film, thereby further enhancing the kinetic performance of thick-coated lithium transition metal phosphate batteries.

[0166] In some implementations, the porosity of the positive electrode film is 14%-28%.

[0167] In this application, the porosity of the positive electrode film can be tested in the following way: Import the cross-sectional scanning electron microscope (SEM) image of the positive electrode film along the electrode thickness direction obtained as described above into ImageJ software. Select the line tool and use a line to mark the length of the scale bar in the image. Click "Analyze Set Scale" and set the scale parameters in the software according to the scale bar length in the image. Select the rectangle tool and select the part of the image outside the scale bar area. Use "Image Duplicate" to copy the selected area and use "Image Type 8bit" to adjust the image format. Select "Analyze Set Measurements" and choose the following five options: "Area", "Mean gray value", "Area Fraction", "Limit to threshold", and "Feret's diameter". Select 3 for "Decimal places". Then, select "Image" - "Adjust" - "Threshold" in sequence, and set 0 and 100 in the selected position of "Threshold". The pore data in the cross-sectional SEM image can then be exported using the Analyze-Measure function. Export using "Image" - "Overlay" - "Flatten" to obtain a pore image; click "Apply" in "Threshold", then click "Analyze" - "Analyze Particles", check the four columns on the left to obtain pore statistics.

[0168] It is understood that in this embodiment, "pores" in the cross-section of the positive electrode film are identified through image color difference and threshold. These "pores" are not the pore data obtained from the degassing test, but are mainly used to characterize the gaps between particles in the cross-section of the positive electrode film. This method is superior to the degassing method because the porosity obtained by the degassing method is related to the pores between particles and the pores in the carbon coating material on the particle surface, and cannot objectively reflect the pores between particles.

[0169] In some embodiments, the porosity of the positive electrode film can be selected as 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, or any value range between the two.

[0170] When the porosity of the positive electrode film is within the aforementioned range, the positive electrode film exhibits good electrolyte wettability and tortuosity, which facilitates the diffusion of lithium ions in both the liquid and solid phases. This helps reduce concentration polarization in thick electrode sheets and improves the battery's kinetic performance. Simultaneously, it helps alleviate volume expansion of thick-coated electrodes during cycling, reduces mechanical stress in the film, and minimizes stress concentration, thereby reducing the risk of film detachment from thick-coated electrodes.

[0171] Especially in thick-coated soft-pack batteries, the gap between the casing and the electrode is small, the volume occupancy of the film is large, the electrolyte capacity is reduced, and the porosity of the positive electrode film is within the above range, which helps to improve the liquid retention rate of the cell and improve the battery dynamic performance.

[0172] In some embodiments, the resistivity of the positive electrode film is 10 Ω·cm to 35 Ω·cm.

[0173] In some embodiments, the resistivity of the positive electrode film is 10 Ω·cm, 12 Ω·cm, 14 Ω·cm, 16 Ω·cm, 18 Ω·cm, 20 Ω·cm, 22 Ω·cm, 22 Ω·cm, 24 Ω·cm, 26 Ω·cm, 28 Ω·cm, 30 Ω·cm, 32 Ω·cm, 35 Ω·cm, or any value between the two.

[0174] Having the resistivity of the positive electrode film within the above range is beneficial for reducing electron transport impedance, minimizing charge-discharge polarization, and improving the rate performance and cycle performance of the battery.

[0175] In some embodiments, the positive electrode film layer further includes a dispersant, including hydrogenated nitrile butadiene rubber (HNBR).

[0176] HNBR is obtained by hydrogenating and saturating the double bonds of nitrile rubber. Its highly saturated main chain structure gives it excellent oil resistance, heat resistance, and aging resistance. This allows it to remain stable in different environments and systems when used as a dispersant, without easily degrading or deteriorating, thus effectively exerting its dispersing effect. The HNBR molecular chain contains both polar nitrile groups and non-polar hydrocarbon segments. The polar nitrile groups can interact with some polar substances or particle surfaces, such as through hydrogen bonding or electrostatic interactions, and adsorb onto the surface of the dispersed particles; the non-polar hydrocarbon segments have good oleophilicity and can extend and disperse well in non-polar or weakly polar media, so that the particles are uniformly dispersed in the medium.

[0177] When HNBR adsorbs onto the surface of particles in the slurry, its long-chain molecules form a physical barrier around the particles, preventing them from approaching each other and agglomerating, thus maintaining a relatively independent dispersion. Simultaneously, HNBR reduces the surface tension between the dispersion medium and the dispersed particles, making the particles easier to wet and promoting dispersion. It also reduces the interfacial energy between particles, minimizing aggregation driven by interfacial energy. Furthermore, during slurry drying and film formation, the elastic network structure of HNBR buffers the shrinkage stress caused by solvent evaporation, reducing the re-agglomeration of conductive agents due to capillary forces, lowering the area of ​​agglomerated regions, and improving the battery's kinetic performance and cycle life.

[0178] In some implementations, the mass content of the dispersant is 0.5%-2% based on the mass of the positive electrode film.

[0179] In some embodiments, based on the mass of the positive electrode film, the mass content of the dispersant can be selected as 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.5%, 2%, or any value range between the two.

[0180] When the mass content of the dispersant is within the above range, it can achieve uniform dispersion of particles in the positive electrode film while maintaining a high loading capacity, reduce stress concentration in the thick-coated lithium transition metal phosphate positive electrode film, and effectively alleviate the problem of battery capacity drop.

[0181] In some embodiments, the positive electrode film layer further includes a conductive agent, and the area of ​​the agglomerated region of the conductive agent accounts for 0.5%-2.5% based on the total area of ​​the cross section of the positive electrode film layer along the thickness direction of the electrode sheet.

[0182] In this application, the area ratio of the conductive agent agglomeration region, based on the total area of ​​the cross-section of the positive electrode film layer along the electrode thickness direction, can be tested using the following method. A similar method to that described above is used to observe the cross-section of the positive electrode film layer along the electrode thickness direction using a scanning electron microscope (SEM), and the area of ​​the conductive agent agglomeration region in the SEM image is measured at 3kx magnification. Since the conductive agent is generally a carbon-based material, such as conductive carbon black or carbon nanotubes, aggregated conductive agent can be seen under high magnification in the SEM. The conductive agent agglomeration region often appears black and agglomerated compared to other areas in the positive electrode film layer. Using image analysis software, the conductive agent agglomeration region refers to the area in the SEM image where the conductive agent is clearly aggregated and appears black. Specifically, the scanning electron microscope (SEM) image at 3kx magnification is imported into ImageJ. Black conductive agent agglomeration regions with a Feret value greater than or equal to 2μm are selected, and the sum of the areas of these selected regions is recorded as the area of ​​the conductive agent agglomeration region. The area ratio of the conductive agent agglomeration region is the ratio of its area to the total area of ​​the imported SEM image. Three randomly selected, non-overlapping SEM images are used, and the average of these ratios is calculated as the "area ratio of the conductive agent agglomeration region based on the total area of ​​the cross-section along the electrode thickness direction of the positive electrode film."

[0183] In some embodiments, the positive electrode film layer further includes a conductive agent, and the area percentage of the agglomerated region of the conductive agent can be selected from 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, or any value range between the two, based on the total area of ​​the cross-section of the positive electrode film layer along the thickness direction of the electrode sheet.

[0184] Based on the total area of ​​the cross-section of the positive electrode film along the thickness direction of the electrode sheet, the area ratio of the agglomeration region of the conductive agent is within the above range, indicating that the conductive agent in the positive electrode film is uniformly dispersed and it is easy to form a uniform conductive network. This is especially beneficial to reduce the problem of kinetic decline caused by the growth of ion transport paths in thick coating films, reduce local polarization and even lithium plating problems generated during battery cycling, and improve the cycle life of the battery.

[0185] Meanwhile, research shows that the first large-sized particles in lithium transition metal phosphate particles are prone to rebound. The agglomeration area of ​​the conductive agent within the above range can suppress the rebound of lithium transition metal phosphate particles by means of the uniform distribution of the conductive agent, forming mechanical constraints on the particles and even the film layer, improving the cohesion of the film layer, reducing the phenomenon of film layer powder shedding and shedding, and improving the cycle life of the battery.

[0186] In some embodiments, the positive electrode film layer further includes a conductive agent, and the area of ​​the agglomerated region of the conductive agent accounts for 1.5%-2.5% based on the total area of ​​the cross section of the positive electrode film layer along the thickness direction of the electrode sheet.

[0187] In this embodiment, the area ratio of the agglomerated region of the conductive agent is further within the above-mentioned range, indicating that the conductive agent is more uniformly distributed in the positive electrode film layer and the content of the conductive agent is low. While improving the dynamic performance of the positive electrode film layer, it helps to reduce the space occupied by the excessive conductive agent on the positive electrode active material, thereby improving the battery's dynamic performance and further increasing the battery's volumetric energy density.

[0188] In some embodiments, the conductive agent includes carbon nanotubes, which include one or more of single-walled carbon nanotubes, few-walled carbon nanotubes, and multi-walled carbon nanotubes.

[0189] In this application, the term "carbon nanotube" refers to a structure composed of carbon atoms arranged in sp... 2 Graphene sheets, formed by hybrid bonding, are rolled up to form nanomaterials with several to dozens of coaxial hollow cylindrical layers. Their diameters typically range from several to tens of nanometers, while their lengths can vary from micrometers to centimeters, exhibiting a high aspect ratio. Based on the number of layers, graphene sheets can be classified into: single-walled carbon nanotubes (SWCNTs), few-walled carbon nanotubes (FWCNTs), and multi-walled carbon nanotubes (MWCNTs). Carbon nanotubes possess excellent electrical conductivity and high elastic modulus.

[0190] Because carbon nanotubes have a one-dimensional structure, they can form a network structure in the positive electrode film. On the one hand, the high elastic modulus of carbon nanotubes enables their network structure to not only act as a bridge for stress propagation but also to bind the thickly coated positive electrode film, suppressing the rebound of lithium-containing transition metal phosphate particles, effectively alleviating stress concentration, reducing the risk of film shedding, and thus improving the problem of battery capacity drop. On the other hand, the excellent conductivity of carbon nanotubes makes their network structure a highly efficient electron transport channel. Even if there is local film shedding, the thick electrode can still maintain high electron transport efficiency in the in-plane and thickness directions, thereby delaying the occurrence of capacity drop and further improving the battery's dynamic performance and cycle life.

[0191] In some embodiments, the conductive agent also includes conductive carbon black.

[0192] Conductive carbon black has a high specific surface area, and thus possesses excellent liquid retention capacity. Thick electrodes generate large expansion force during cycling, which makes the electrolyte prone to being squeezed out. The distribution of conductive carbon black in the positive electrode film layer is beneficial to improving the liquid retention capacity of the thick electrode, further alleviating the phenomenon of capacity plunge of the battery during cycling, and improving the cycle life of the battery.

[0193] In some embodiments, the agglomerated region of the conductive agent includes carbon nanotubes and conductive carbon black.

[0194] The researchers found that carbon nanotubes are prone to agglomeration due to their high surface energy, resulting in uneven dispersion in the positive electrode film layer and failure to form an effective carbon nanotube network structure. Conductive carbon black and carbon nanotubes have relatively close surface energies, and can be adsorbed on the surface of carbon nanotubes to form a physical barrier, increase the resistance to agglomeration of carbon nanotubes, reduce direct contact between carbon nanotubes, and thereby inhibit the agglomeration phenomenon, improving the distribution uniformity of carbon nanotubes in the positive electrode film layer. On the one hand, this helps improve the conductivity of the thickly coated positive electrode film layer and enhance the kinetic performance of the battery; on the other hand, it helps exert the binding effect of carbon nanotubes on the positive electrode film layer, reduce the risk of peeling of the thickly coated positive electrode film layer, and further improve the kinetic performance and cycle life of the battery. In addition, the agglomeration of carbon nanotubes in the agglomerated region of the conductive agent will also cause local ion transport paths in the agglomerated region of the conductive agent to be blocked. The matching of conductive carbon black can improve the lithium ion transport capacity in this region, reduce local polarization, and further improve the cycle stability of the battery. In some embodiments, based on the mass of the positive electrode film layer, the mass content C1 of the carbon nanotubes satisfies: 0<C1≤2.5%, and the mass content C2 of the conductive carbon black satisfies: 0<C2≤2.5%.

[0195] In some embodiments, based on the mass of the positive electrode film layer, the mass content C1 of the carbon nanotubes can be selected as 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5% or any numerical range between the two.

[0196] In some embodiments, based on the mass of the positive electrode film layer, the mass content C2 of the conductive carbon black can be selected as 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5% or any numerical range between the two.

[0197] When the mass content of carbon nanotubes and conductive carbon black is within the above range, it can effectively alleviate the aggregation of carbon nanotubes and form a good conductive network structure, thereby effectively reducing the stress concentration of the positive electrode film and improving the liquid retention rate of the positive electrode during long-term cycling. This further reduces the risk of electrode film shedding and polarization, improves the dynamic performance of the battery, and also addresses the capacity drop problem and improves the cycle life of the battery.

[0198] In some embodiments, the battery cell further includes a separator 20 disposed between the positive electrode and the negative electrode. The separator 20 includes a base film 201, a ceramic layer 202 disposed on at least one side of the base film 201, and an adhesive layer 203 disposed on the side of the ceramic layer 202 away from the base film 201. The adhesive layer 203 is a continuous layer with a porous structure and includes a vinylidene fluoride polymer.

[0199] In some embodiments, the battery cell further includes a separator disposed between the positive electrode and the negative electrode. The separator includes a base film, ceramic layers disposed on both sides of the base film, and an adhesive layer disposed on at least one side of the ceramic layer away from the base film.

[0200] Placing ceramic layers on both sides of the base film helps improve the rigidity of the pouch cell and reduces local stress concentration.

[0201] In some embodiments, the battery cell further includes a separator disposed between the positive electrode and the negative electrode. The separator includes a base film, ceramic layers disposed on both sides of the base film, and an adhesive layer disposed on the ceramic layers on the sides away from the base film.

[0202] In some embodiments, the vinylidene fluoride polymer includes one or more of polyvinylidene fluoride (PVDF) and polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP).

[0203] In some embodiments, vinylidene fluoride polymers include polyvinylidene fluoride (PVDF).

[0204] In the prior art, the adhesive layer of the separator usually uses aqueous PVDF, which presents an island-like structure in the separator, as shown in Figure 2. This is beneficial for providing gaps for cell expansion and is also convenient for manufacturing; however, such a separator adhesive layer has a small contact area with the electrode and weak adhesion.

[0205] The diaphragm provided in this application uses a continuous porous layer as the adhesive layer, as shown in Figures 1 and 3. Compared with the adhesive layer in the prior art, it has a larger bonding area with the electrode, which makes the bonding between the diaphragm and the electrode more firm and uniform. Furthermore, when the positive electrode film layer rebounds, it helps to maintain the interfacial contact between the diaphragm and the positive electrode film layer, reducing the probability of film layer detachment.

[0206] It is understandable that a continuous adhesive layer may break and deform into a blocky structure during electrode manufacturing or cycling due to contact with or compression of the positive or negative electrode. The continuous structure referred to in this application means that, at the microscopic level, such as under a scanning electron microscope or optical microscope, the adhesive layer of the separator is continuous. To reflect the true morphology of the separator, during sampling, it is preferable to sample in areas of the battery where the separator's adhesive layer is not bonded to the positive or negative electrode. For example, sampling can be performed at locations beyond the positive and negative electrode; or sampling can be performed near the surface of the electrode assembly. This sampling area has less adhesion to the positive or negative electrode, providing a better reflection of the separator's true state.

[0207] Compared to wound cells, laminated cells have less compression between the separator and the electrode, making them more prone to relative displacement. This displacement can disturb the membrane layer, leading to powder shedding or detachment. Furthermore, it can cause the positive and negative electrodes to overlap, increasing the risk of internal short circuits within the cell. Therefore, the separator provided in this application is particularly suitable for laminated cells. Increased adhesion between the porous adhesive layer and the electrode helps improve the bond between the separator and the electrode, reducing relative displacement. This helps reduce disturbance to the positive electrode membrane layer, lowering the probability of membrane detachment, and also reduces the risk of short circuits caused by positive and negative electrode overlap.

[0208] In summary, when the vinylidene fluoride polymer in the adhesive layer of this application is selected from the above-mentioned materials, it helps to form a continuous and uniform porous adhesive layer. First, the adhesion between the adhesive layer and the electrode is improved and uniformly distributed, which helps to reduce stress concentration in the thick-coated lithium transition metal phosphate positive electrode film, reducing the risk of film detachment and thus helping to further improve the cycle life of the battery. Second, the stable adhesion between the adhesive layer and the positive or negative electrode helps to reduce the direct contact between the positive and negative electrode due to the relative displacement between the electrode and the separator, reducing the risk of internal short circuit and helping to improve battery safety performance. Third, the porous adhesive layer helps to maintain the porosity of the separator, reserving space for cell expansion and further improving the cycle life of the battery.

[0209] In some embodiments, the base film may be made of one or more of the following materials, including but not limited to glass fiber, nonwoven fabric, polyethylene (PE), and polypropylene (PP).

[0210] In some embodiments, the ceramic layer includes one or more of alumina (Al2O3), zirconium oxide (ZrO2), titanium oxide (TiO2), silicon oxide (SiO2), and boron nitride (BN).

[0211] Ceramic particles possess flame retardancy and high hardness, making them resistant to deformation under heat and exhibiting excellent dimensional stability. The low thermal conductivity of ceramic materials further prevents certain thermal runaway points in the battery from expanding into overall thermal runaway, thereby improving the safety performance of individual battery cells.

[0212] In some implementations, the thickness of the base membrane in the diaphragm is 7-9 μm.

[0213] In some embodiments, the thickness of the base film in the diaphragm can be selected as 7 μm, 7.5 μm, 8 μm, 8.5 μm, 9 μm or any value range between the two.

[0214] In some embodiments, the thickness of the ceramic layer in the diaphragm is 2-4 μm on one side.

[0215] In some embodiments, the thickness of the ceramic layer on one side of the diaphragm can be selected as 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm or any value range between the two.

[0216] In some embodiments, the thickness of the adhesive layer on one side of the diaphragm is 1-5 μm.

[0217] In some embodiments, the thickness of the adhesive layer on one side of the diaphragm can be selected as 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm or any value range between the two.

[0218] In this application, "thickness" has a meaning known in the art and can be measured using methods and instruments known in the art. As an example, a high-precision micrometer (e.g., Mitutoyo 293-100 model, with an accuracy of 0.1 μm) can be used for testing.

[0219] If the adhesive layer is too thin, the void space in the separator is small and the adhesion between the separator and the electrode is weak. On the one hand, the stress increases after the membrane expands, increasing the probability of membrane detachment and affecting the cycle life of the battery; on the other hand, the probability of a short circuit between the positive and negative electrodes increases, thus affecting the battery's safety performance. If the adhesive layer is too thick, it occupies a large amount of space in the battery, thus affecting the battery's volumetric energy density. In the embodiments of this application, the thickness of the adhesive layer is within the above-mentioned range, which helps to balance the battery's cycle life, safety performance, and volumetric energy density.

[0220] In some embodiments, the positive electrode film layer has an undercoat layer in the bottom region near the positive electrode current collector. The undercoat layer includes a conductive agent and a binder. The conductive agent includes carbon nanotubes and conductive carbon black, and the binder includes polyvinylidene fluoride (PVDF).

[0221] In some embodiments, the thickness of the base coating is 0.5 μm to 5 μm.

[0222] In some embodiments, the thickness of the base coating can be selected as 0.5 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm or any value range between the two.

[0223] The undercoating layer provided in this application helps improve the adhesion between the positive electrode film and the positive electrode current collector and alleviates stress concentration at large particles, thereby reducing the probability of positive electrode film detachment and improving the cycle stability of the battery. Simultaneously, compared to direct contact between the positive electrode current collector and the positive electrode film, the increased contact area between the undercoating layer and the positive electrode film helps increase the area for electron transport between the current collector and the positive electrode film, thereby reducing the internal resistance of the electrode and improving the battery's dynamic performance.

[0224] In some embodiments, as shown in FIG4, the battery cell 5 includes a housing 50, and the stacked cells are housed within the housing 50. The housing 50 has a dimension L0 in the length direction X, a dimension W0 in the width direction Y, and a dimension H0 in the thickness direction Z, wherein 480mm≤L0≤720mm, 100mm≤W0≤150mm, and 14mm≤H0≤22mm.

[0225] In some implementations, L0 can be selected as 480mm, 490mm, 500mm, 510mm, 520mm, 530mm, 540mm, 550mm, 560mm, 570mm, 580mm, 590mm, 600mm, 610mm, 620mm, 630mm, 640mm, 650mm, 660mm, 670mm, 680mm, 690mm, 700mm, 710mm, 720mm, 750mm, 800mm, 850mm, 900mm, 950mm, 1000mm, 1050mm, 1100mm, 1150mm, 1200mm, 1250mm, 1300mm, or any value range between the two.

[0226] In some implementations, W0 can be selected as 100mm, 110mm, 120mm, 130mm, 140mm, 150mm or any value range between the two.

[0227] In some implementations, H0 can be selected as 14mm, 15mm, 16mm, 17mm, 18mm, 19mm, 20mm, 21mm, 22mm or any value range between the two.

[0228] In some embodiments, the length dimension of the housing is L0, where 450mm≤L0≤650mm.

[0229] When the length dimension L0 of the casing satisfies 450mm≤L0≤650mm, the length of the battery cell is shorter, which helps to shorten the current diffusion path, reduce the internal resistance of the electrode, thereby reducing the heat generation of the battery and improving its dynamic performance. In addition, the shorter casing length helps to shorten the diffusion path of the electrolyte during the wetting process, improve the wetting rate and uniformity of the electrolyte, further promote the uniformity of lithium ion insertion and extraction during cycling, alleviate stress concentration, reduce the risk of film peeling, and improve the cycle stability of the battery cell.

[0230] In some embodiments, the length dimension of the housing is L0, where 900mm ≤ L0 ≤ 1300mm.

[0231] When the length dimension L0 of the casing satisfies 900mm ≤ L0 ≤ 1300mm, the battery cell is relatively long. This helps reduce the volume ratio of the casing within the battery cell and increase the load ratio of active materials. Simultaneously, a longer battery cell can reduce the number of batteries required within the battery module, simplifying the module's structural design and reducing the number and complexity of structural components. This improves the space utilization of the battery pack and ultimately contributes to increasing the volumetric energy density of the battery cells.

[0232] In some embodiments, as shown in FIG4, the material of the housing 50 is a soft-pack material, which includes an aluminum-plastic composite film, optionally including one or more of polypropylene (PP), polybutylene terephthalate (PBT), polybutylene succinate (PBS), nylon, polyethylene terephthalate (PET), and polyethylene (PE) forming a composite film with aluminum.

[0233] The applicant discovered that pouch cells are lighter than rigid casings such as aluminum and steel, which is beneficial for further improving the energy density of lithium transition metal phosphate batteries. Furthermore, pouch cells have higher elongation, resulting in thinner and more flexible casings that improve space utilization of individual battery cells, thereby increasing their energy density. Additionally, aluminum's high barrier properties effectively reduce the penetration of water and oxygen into the battery, decreasing electrolyte decomposition and electrode material oxidation, thus extending battery life.

[0234] In some embodiments, continuing to refer to FIG4, the housing 50 includes a first sealing area 51, which is disposed at at least one end of the laminated cell extending in the width direction; the first sealing area 51 includes a folded edge structure extending in the length direction, on which encapsulating adhesive is disposed, and the encapsulating adhesive is continuously disposed in the length direction and fixes the folded edge structure.

[0235] A folded edge structure refers to a reinforced structure formed by folding the encapsulation area in half. There is no limit to the number of folds. As an example, it can be a single folded edge structure with one fold or a double folded edge structure with folds on both sides.

[0236] During electrode cycling, the SEI film thickens, leading to significant rebound and gas generation during long cycles. The sealing area of ​​the pouch cell is used to seal the electrode assembly, but the sealing area has limited strength and is easily broken open by the large rebound and high gas generation within the film.

[0237] This application embodiment further enhances the sealing strength of the first sealing area by including a folded edge structure extending along the length direction. The continuous arrangement of the encapsulating adhesive along the length direction and the fixing of the folded edge structure, compared to a discontinuous arrangement of the encapsulating adhesive along the length direction, further improves the sealing strength, achieving continuous reinforcement of the sealing area along its length and reducing the probability of the thick-coated electrode breaking open the sealing area in the packaging during cycling.

[0238] In some embodiments, the housing 50 includes at least one second sealing area 52, which is disposed along the length of the housing at at least one end of the laminated cell, and the second sealing area 52 is disposed on the tab side of the laminated cell.

[0239] It is understandable that the positive and negative electrodes can be located on the same side of the laminated cell, as shown in Figure 1; or they can be located on opposite sides of the laminated cell.

[0240] In some embodiments, the battery cell 5 further includes a lead 53 connected to the tab of the battery cell. For example, the lead 53 can be soldered to the tab. The lead 53 is a conductive element, and at least a portion of the lead 53 is located outside the housing 50. The lead 53 serves as the electrode lead-out end of the battery cell 5, facilitating electrical connection between the battery cell 5 and other battery cells 5 or other components. For example, the lead 53 can be in the form of a sheet.

[0241] Correspondingly, lead-out element 53 also includes a positive lead-out element and a negative lead-out element, with the positive lead-out element connected to the positive electrode tab and the negative lead-out element connected to the negative electrode tab.

[0242] In some implementations, the second sealing area is located on the tab side. The tab needs to be connected to the lead-out component. The connection strength between the lead-out component and the casing material is relatively weak, which makes it easier for gas to escape from the second sealing area. This is beneficial for directional pressure relief of the battery, reducing the impact on adjacent cells during thermal runaway, and improving the overall service life of the battery.

[0243] In some embodiments, the outer periphery of the laminated cell is provided with a plurality of rubber rings that surround in the width direction, and the rubber rings that surround in the width direction are spaced apart in the length direction.

[0244] The rubber rings that wrap around the width of the cell and are spaced apart along the length help to fix the position between the electrodes in the cell, reducing the probability of cell displacement during battery shaking. This is especially suitable for batteries with a large length, as it can effectively reduce the mutual displacement between the electrodes in the length direction, thus reducing lithium plating. This helps to maintain the stability of the internal spatial structure of the battery, thereby not affecting the normal operation of the battery.

[0245] In some embodiments, the capacity of the battery cell is 95Ah-300Ah at 25°C.

[0246] In some embodiments, the capacity of the battery cell is 150Ah-180Ah at 25°C.

[0247] In this application, the capacity of a single battery cell has a meaning known in the art and can be tested using methods known in the art. As an example, at 25°C, the battery is charged to 3.65V at a charging rate of 0.5C (the nominal capacity), then charged at a constant voltage of 3.65V to 0.05C, left to stand for 10 minutes, and then discharged to 2.5V at a discharging rate of 1C, left to stand for 10 minutes. The capacity C during the discharge process is calculated using the formula C = I*t, with the unit being Ah.

[0248] In some embodiments, at 25°C, the capacity of the battery cell can be selected as 95Ah, 100Ah, 105Ah, 107Ah, 110Ah, 115Ah, 120Ah, 125Ah, 130Ah, 135Ah, 140Ah, 145Ah, 150Ah, 155Ah, 160Ah, 161Ah, 162Ah, 163Ah, 164Ah, 165Ah, 170Ah, 175Ah, 180Ah, 182Ah, 185Ah, 190Ah, 200Ah, 210Ah, 220Ah, 230Ah, 240Ah, 250Ah, 270Ah, 280Ah, 290Ah, 300Ah, or any value range between the two.

[0249] In some embodiments, the positive current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer substrate and a metal layer formed on at least one surface of the polymer substrate. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0250] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer substrate and a metal layer formed on at least one surface of the polymer substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0251] In some embodiments, the negative electrode film layer includes a negative electrode active material. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, and hard carbon. However, this application is not limited to these materials, and other conventional materials that can be used as battery negative electrode active materials may also be used. These negative electrode active materials may be used alone or in combination of two or more.

[0252] In some embodiments, the negative electrode film layer may optionally include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0253] In some embodiments, the negative electrode film may optionally include other additives, such as thickeners (e.g., sodium carboxymethyl cellulose (CMC-Na)).

[0254] In some embodiments, the negative electrode sheet can be prepared by dispersing the components used to prepare the negative electrode sheet, such as the negative electrode active material, conductive agent, binder and any other components, in a solvent (e.g., deionized water) to form a negative electrode slurry; coating the negative electrode slurry onto the negative electrode current collector, and then obtaining the negative electrode sheet after drying, cold pressing and other processes.

[0255] A second aspect of this application provides a battery device, including the battery cell provided in the first aspect of this application.

[0256] The battery device disclosed in this application can be used in electrical devices that use the battery device as a power source or in various energy storage systems that use the battery device as an energy storage element. Besides vehicles, the battery device can also be used in, but is not limited to, mobile phones, tablets, laptops, electric toys, power tools, electric vehicles, electric cars, ships, spacecraft, etc. Electric toys can include stationary or mobile electric toys, such as game consoles, electric car toys, electric ship toys, and electric airplane toys, etc. Spacecraft can include airplanes, rockets, space shuttles, and spacecraft, etc.

[0257] A third aspect of this application provides an electrical device that uses a battery as a power source, the electrical device including at least one of the battery cell, battery module, or battery pack provided in this application. The battery cell, battery module, or battery pack can be used as a power source for the electrical device, or as an energy storage unit for the electrical device. The battery cell, battery module, or battery pack can be selected as the electrical device according to its usage requirements.

[0258] Figure 5 shows an example of an electrical device. The electrical device disclosed in this application can be a gasoline-powered vehicle, a natural gas-powered vehicle, or a new energy vehicle. New energy vehicles can be pure electric vehicles, hybrid electric vehicles, or range-extended electric vehicles, etc. A battery device is installed inside the vehicle, and the battery device can be located at the bottom, front, or rear of the vehicle. The battery device can be used to power the vehicle; for example, the battery device can serve as the vehicle's operating power source. The vehicle may also include a controller and a motor. The controller is used to control the battery device to supply power to the motor, for example, for the vehicle's starting, navigation, and operating power needs. In some embodiments of this application, the battery device can not only serve as the vehicle's operating power source but also as the vehicle's driving power source, replacing or partially replacing gasoline or natural gas to provide driving power to the vehicle.

[0259] The fourth aspect of this application provides an energy storage device that uses a battery device as a power source. The energy storage device can be, but is not limited to, an energy storage container, an energy storage cabinet, an energy storage power station, an energy storage battery pack, or a portable energy storage system.

[0260] Example

[0261] The following describes embodiments of this application. The embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.

[0262] Example 1

[0263] (1) Preparation of positive electrode active material

[0264] Lithium dihydrogen phosphate, ferrous oxalate, carbon source, titanium dioxide, and vanadium pentoxide were mixed evenly in methanol and ground to obtain a mixed raw material. The ratio of lithium dihydrogen phosphate to ferrous oxalate was such that the molar ratio of lithium to iron was 1.025:1.0. The carbon source consisted of polyethylene glycol with a weight average molecular weight of 500, polyethylene glycol with a weight average molecular weight of 2000, and polyethylene glycol with a weight average molecular weight of 4000, all in a mass ratio of 2:6:2. The particle size D of the ferrous oxalate was... 10 With a particle size of 6.5 μm and a diameter D 50 62μm, particle size D 90 The thickness is 108 μm, and the mass content of Fe in ferrous oxalate is 30.5%, while the mass content of ferric iron is 0.03%.

[0265] The mixed raw materials are ball-milled multiple times and demagnetized in a ball mill to obtain a mixed slurry. The number of grinding cycles and time are controlled, and the particle size Dv of the resulting mixed slurry is determined. 50 It is 3.15μm.

[0266] The spray-dried slurry yields a dried precursor powder, which is light yellow in appearance and uniform in color.

[0267] The precursor powder was placed in a sintering furnace and heated from 25°C to 360°C at a rate of 2°C / min under a nitrogen atmosphere, and held at that temperature for 3.5 h. Then, the temperature was increased to a second temperature of 785°C at a rate of 5°C / min and held at that temperature for 10 h. Afterward, the material was cooled. Based on the total mass of the positive electrode active material, the Ti element content was 1050 ppm and the V element content was 950 ppm.

[0268] The obtained material was crushed using an airflow pulverization method with a staged frequency of 21 Hz and a pulverizing airflow of 0.54 MPa to obtain carbon-coated lithium iron phosphate cathode active material.

[0269] The D10, D50, D90, and Dv50 mentioned above refer to the data obtained by testing using the Malvern laser scattering method.

[0270] (2) Preparation of positive electrode sheet

[0271] The above-mentioned positive electrode active material, conductive agent, and binder polyvinylidene fluoride were mixed in a mass ratio of 94.1:1.9:3 in the solvent N-methylpyrrolidone. Then, 1% by mass of dispersant HNBR was added, and the mixture was thoroughly mixed, stirred, and dispersed in a stirring tank to form a positive electrode slurry. After the stirring process was completed, the positive electrode slurry was transported to the coating process. The conductive agent included conductive carbon black and multi-walled carbon nanotubes in a mass ratio of 0.9:1, and the specific surface area of ​​the conductive carbon black was 80 m². 2 / g, oil absorption value of 180mL / 100g, average length of carbon nanotubes of 20μm, specific surface area of ​​280m². 2 / g;

[0272] The positive electrode slurry was extruded onto aluminum foil, dried, and then cold-pressed to obtain a positive electrode film with a single-sided thickness H of 105.64 μm and a compaction density of 2.36 g / cm³. 3 The positive electrode sheet. Here, compaction density refers to the compaction density of a single battery cell under full discharge conditions.

[0273] The positive electrode sheets are slit and punched into specified shapes, and then the punched positive electrode sheets are sorted by weight using a weighing and sorting machine for stacking by a stacking machine.

[0274] Among them, in the cross-section of the positive electrode film along the electrode thickness direction, in the cumulative distribution curve of the spheroidal area of ​​particles with particle size R1 satisfying R1≥1000nm, the median L of spheroidality is... R1A50 The median C of the graphitization degree of the positive electrode film is 0.72. 50 The concentration of graphitization degree C is 1.12; 90 -C 10 ) / C 50 The value is 0.025; based on the total area of ​​particles in the cross-section along the thickness direction of the positive electrode film, the area ratio of particles with a particle size R1 satisfying R1≥1000nm is 35.28%; the median value B of the positive electrode film coating value is 0.025. 50 The value is 0.441; the iron dissolution rate of the positive electrode material is 976 ppm; based on the total area of ​​the cross-section of the positive electrode film along the thickness direction of the electrode sheet, the area ratio of the agglomeration region of the conductive agent is 1.91%; the porosity of the positive electrode film is 15.06%; and the film resistivity of the positive electrode film is 31.0 Ω·cm.

[0275] (2) Preparation of negative electrode sheet

[0276] A mixture of artificial graphite and natural graphite (by weight 1:1), conductive carbon black (as a conductive agent), styrene-butadiene rubber (SBR) (as a binder), and sodium carboxymethyl cellulose (CMC) (as a thickener) are mixed evenly in a weight percentage of 96:0.5:2.0:1.5. Deionized water is then added, and the mixture is stirred and dispersed to obtain a negative electrode slurry. The negative electrode slurry is then coated onto a copper foil substrate, and after drying, cold pressing, slitting, and sheet forming, a negative electrode sheet is obtained.

[0277] The negative electrode sheets are slit and punched into specified shapes, and then the punched negative electrode sheets are sorted by weight using a weighing and sorting machine for stacking by a stacking machine.

[0278] (3) Diaphragm

[0279] Polyvinylidene fluoride (PVDF) was dissolved in N-methylpyrrolidone (NMP) and stirred until homogeneous. Polyethylene glycol (PEG) was then added as a pore-forming agent and thoroughly mixed to obtain an adhesive layer solution. This adhesive layer solution was applied to the aforementioned base membrane with ceramic layers on both sides. After pre-evaporation at 80°C and drying at 110°C, the membrane was immersed in deionized water to dissolve the PEG, resulting in a membrane with a porous adhesive layer.

[0280] The thickness of the base film is 8 μm, the thickness of the single-sided ceramic layer is 3 μm, and the thickness of the single-sided adhesive layer is 1 μm.

[0281] (4) Electrolyte

[0282] In an argon atmosphere glove box (H2O < 0.1 ppm, O2 < 0.1 ppm), organic solvents dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), and ethylene carbonate (EC) are mixed evenly.

[0283] Lithium hexafluorophosphate was then added and dissolved in an organic solvent to achieve a concentration of 1.05 mol / L. Ethylene carbonate (VC) was then added and stirred until homogeneous to obtain the electrolyte of Example 1.

[0284] Based on the total mass of the electrolyte, the mass content of dimethyl carbonate is 26%, the mass content of ethyl methyl carbonate is 43.3%, the mass content of ethylene carbonate is 17.3%, and the mass content of vinylene carbonate is 0.9%.

[0285] (5) Battery fabrication:

[0286] The positive electrode, separator, and negative electrode are stacked in sequence using a stacking machine. The separator must effectively isolate the positive and negative electrodes to obtain a stacked battery cell. The stacked battery cell is then coated with adhesive to ensure tight coverage. The coated stacked battery cell is placed in an outer packaging material, an aluminum-plastic film, which is composed of an inner polypropylene layer, a middle aluminum foil layer, and an outer nylon composite layer. The aluminum-plastic film outer packaging is then formed and trimmed using a punching machine to obtain the target shape and size. The aluminum-plastic film is then heat-sealed to ensure a sealing tensile strength ≥25N / 8mm. The battery undergoes vacuum baking, settling, electrolyte injection, and sealing. Finally, the soft-pack battery is subjected to hot and cold pressing operations. The hot pressing temperature is 45℃, the time is 2 minutes, and the pressure is 90kg / cm². 2 The cold pressing temperature was 25℃, the time was 2 minutes, and the pressure was 90 kg / cm². 2 Finally, after processes such as formation, vacuum degassing, and edge trimming, the battery cell is obtained. The battery cell has a length of 600mm, a width of 125mm, and a thickness of 20mm.

[0287] The preparation methods of Examples 2-10 are basically the same as those of Example 1, except that the preparation method of the positive electrode active material is adjusted, as follows:

[0288] Example 2

[0289] The preparation method of Example 2 is basically the same as that of Example 1, except that the second temperature is adjusted to 765°C in the preparation of the positive electrode active material.

[0290] Example 3

[0291] The preparation method of Example 3 is basically the same as that of Example 1, except that the second temperature is adjusted to 735°C in the preparation of the positive electrode active material.

[0292] Example 4

[0293] The preparation method of Example 4 is basically the same as that of Example 1, except that in the preparation of the positive electrode active material, the carbon source is replaced with polyethylene glycol with a weight average molecular weight of 500 and a weight average molecular weight of 2000 in a mass ratio of 2:8.

[0294] Example 5

[0295] The preparation method of Example 5 is basically the same as that of Example 1, except that in the preparation of the positive electrode active material, the carbon source is replaced with polyethylene glycol with a weight average molecular weight of 500.

[0296] Example 6

[0297] The preparation method of Example 6 is basically the same as that of Example 1, except that in the preparation of the positive electrode active material, the carbon source is replaced with polyethylene glycol with a weight average molecular weight of 2000.

[0298] Example 7

[0299] The preparation method of Example 7 is basically the same as that of Example 3, except that in the preparation of the positive electrode active material, the carbon source is replaced with polyethylene glycol and glucose with a mass ratio of 2:8 and a weight average molecular weight of 500.

[0300] Example 8

[0301] The preparation method of Example 8 is basically the same as that of Example 1. The difference is that, in the preparation of the positive electrode sheet, the coating weight is adjusted, and parameters such as the hot roller pressure, hot roller temperature, transfer coating speed, and heating temperature before the first entry into the hot roller for compaction are adjusted accordingly, thereby adjusting the compaction density of the positive electrode sheet.

[0302] Example 9

[0303] The preparation method of Example 9 is basically the same as that of Example 1. The difference is that when preparing the positive electrode sheet, the coating weight is adjusted so that the single-sided thickness H of the positive electrode film layer obtained by cold pressing is 119.12 μm; and the thickness of the battery is appropriately adjusted while keeping the number of positive electrode sheets, separator and negative electrode sheets unchanged.

[0304] Example 10

[0305] The preparation method of Example 10 is basically the same as that of Example 1. The difference is that when preparing the positive electrode sheet, the coating weight is adjusted so that the single-sided thickness H of the positive electrode film layer obtained by cold pressing is 71.53 μm; and the thickness of the battery is appropriately adjusted while keeping the number of positive electrode sheets, separator and negative electrode sheets unchanged.

[0306] Comparative Example 1

[0307] The preparation method of Comparative Example 1 is basically the same as that of Example 7, except that the carbon source is replaced with glucose in the preparation of the positive electrode active material.

[0308] Test method:

[0309] 1. Capacity of a single lithium-ion secondary battery cell

[0310] At 25℃, charge the battery to 3.65V at a charging rate of 0.5C (the nominal capacity), then charge it to 0.05C at a constant voltage of 3.65V, let it stand for 10 minutes, and then discharge it to 2.5V at a discharging rate of 1C, let it stand for 10 minutes. Calculate the capacity C during the discharge process using the formula C=I*t, with the unit being Ah.

[0311] 2. Number of cycles corresponding to 80% capacity decay

[0312] At 25°C, charge the battery to 3.65V at a charging rate of 0.5C (the nominal capacity), then charge it to 0.05C at 3.65V, let it stand for 10 minutes, and then discharge it to 2.5V at a discharging rate of 1C, let it stand for 10 minutes. One charge-discharge cycle is one cycle. Continue the test until the battery capacity decreases to 80% of the nominal capacity. This number of cycles is recorded as the number of cycles @ 80% SOH.

[0313] Test Results

[0314] The test results of the above embodiments and comparative examples are shown in Table 1.

[0315] Table 1. Preparation parameters for each embodiment and comparative example.

[0316] As can be seen from the comparison between Examples 1-10 and Comparative Example 1, the battery cell includes a stacked cell, which includes a positive electrode and a negative electrode. The positive electrode includes a positive current collector and a positive electrode film layer disposed on at least one side of the positive current collector. The positive electrode film layer includes lithium-containing transition metal phosphate particles with carbon material disposed on at least a portion of its surface. In the cumulative distribution curve of the graphitization degree C value obtained by laser microscopy confocal Raman spectroscopy in surface scanning mode, the median C of the graphitization degree is... 50 The value ranges from 0.95 to 1.20, where the degree of graphitization C is I. G / I D I G This indicates that the Raman spectrum is at 1580±100 cm⁻¹ -1 The intensity of peak G at I D This indicates that the Raman spectrum is at 1350±100 cm⁻¹ -1 The intensity of peak D at the specified location indicates that, under fully discharged conditions, the compaction density of the positive electrode sheet is 2.3 g / cm³. 3 -2.6g / cm 3 While maintaining good capacity, individual battery cells help improve cycle life during long-term battery cycles.

[0317] A comparison of Examples 1, 4-6, and 7 shows that the median C of the graphitization degree C in the cumulative distribution curve of the positive electrode film obtained by laser microscopy confocal Raman spectroscopy instrument scanning mode is the highest. 50 Further, it can be selected as 1.01-1.13, which helps to further improve the cycle life of battery cells during long-term cycling.

[0318] As can be seen from the comparison between Examples 1-10 and Comparative Example 1, in the cumulative distribution curve of graphitization degree C value obtained by laser microscopy confocal Raman spectroscopy in the instrument scanning mode, the concentration of C value (C) is higher than that of Comparative Example 1. 90 -C 10 ) / C 50 A value of 0.01-0.05 helps to further improve the cycle life of individual battery cells during long-term cycling.

[0319] As can be seen from Examples 1-3, in the cross-section of the positive electrode film along the thickness direction of the positive electrode sheet, in the cumulative distribution curve of the spheroidal area of ​​particles with a particle size R1 satisfying R1≥1000nm, L R1A50 Within the range of 0.67-0.75, the battery cells exhibit good cycle life during long-term cycling.

[0320] As can be seen from Examples 1-9, when the thickness H of the positive electrode film is in the range of 70μm-120μm, the battery cell can maintain good capacity while helping to improve the cycle life during long-term cycling.

[0321] It should be noted that this application is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this application are included in the technical scope of this application. Furthermore, various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing by combining some of the constituent elements of the embodiments, without departing from the spirit of this application, are also included in the scope of this application.

Claims

1. A battery cell, characterized in that, comprising a laminated cell, wherein the laminated cell comprises a positive electrode plate and a negative electrode plate, the positive electrode plate comprises a positive current collector and a positive electrode film layer disposed on at least one side of the positive current collector, and the positive electrode film layer comprises lithium-containing transition metal phosphate particles at least part of the surface of which is provided with a carbon material, In the cumulative distribution curve of the graphitization degree C value of the positive electrode film obtained in the laser microscopy confocal Raman spectroscopy instrument scanning mode, the median C of the graphitization degree is... 50 The value is 0.95-1.

20. wherein the graphitization degree C value is I G / I D , I G represents the G peak intensity of the Raman spectrum at 1580±100 cm -1 -1, I D represents the D peak intensity of the Raman spectrum at 1350±100 cm -1 -1, The battery cell in full discharge state, the compaction density of the positive pole piece is 2.3g / cm 3 -2.6g / cm 3 .

2. The battery cell according to claim 1, characterized in that, The graphitization degree C value cumulative distribution curve of the positive electrode film layer obtained under the laser microscope confocal Raman spectrometer surface scanning mode, the median number C of the graphitization degree is 1.01-1.

13. 50 1.01-1.

13.

3. The battery cell according to claim 1 or 2, characterized in that, The concentration of C values ​​(C0.05) in the cumulative distribution curve of graphitization degree C values ​​obtained by laser microscopy confocal Raman spectroscopy instrument scanning mode of the positive electrode film is shown in the curve. 90 -C 10 ) / C 50 The value is 0.01-0.05, and can be selected as 0.02-0.

04.

4. The battery cell according to any one of claims 1 to 3, characterized in that, based on the total area of the particles in the cross section of the positive electrode film layer along the thickness direction of the electrode plate, the area proportion of particles with a particle size R1 satisfying R1≥1000 nm is 12%-50%, optionally 12%-40%.

5. The battery cell according to any one of claims 1 to 4, characterized in that, In the cross-section of the positive electrode film along the electrode thickness direction, in the cumulative distribution curve of the sphericity area of ​​the particles with particle size R1 satisfying R1≥1000nm, the median L of the sphericity is... R1A1 50 is 0.6-0.8, can be selected as 0.65-0.75, and can be further selected as 0.67-0.

75.

6. The battery cell according to any one of claims 1 to 5, characterized in that, In the cumulative distribution curve of the coating value B obtained by laser microscopy confocal Raman spectroscopy in instrument scanning mode, the median B of the coating value B is... 50 The value is 0.30-0.

60. Where the coating value B is I P / I D , where I P This indicates that the Raman spectrum is at 948±100 cm⁻¹ -1 The intensity of the P peak at I D This indicates that the Raman spectrum is at 1350±100 cm⁻¹ -1 The intensity of peak D at that location.

7. The battery cell according to any one of claims 1 to 6, characterized in that, The lithium-containing transition metal phosphate particles comprise components represented by the following general formula: Li m Fe x P y O j Q q Formula I, wherein Q is one or more selected from Al, Na, K, Mg, Cu, Mn, Cr, Zn, Pb, Ca, Co, Ni, Sr, Nb, V, Ti, B, S, Si, N, F, Cl, Br, 0.8≤m≤1.15, 0.9≤x≤1, 0.95≤y≤1, 3.5≤j≤4, 0≤q≤0.

1.

8. The battery cell according to any one of claims 1 to 7, characterized in that, The iron dissolution rate of the positive electrode active material is 658ppm-1921ppm, optionally 658ppm-1485ppm.

9. The battery cell according to any one of claims 1 to 8, characterized in that, Based on the total mass of the lithium-containing transition metal phosphate particles, the mass content of titanium element is 500ppm-8000ppm, optionally 1000ppm-3000ppm.

10. The battery cell according to any one of claims 1 to 9, characterized in that, Based on the total mass of the lithium-containing transition metal phosphate particles in the positive electrode film layer, the mass content of vanadium element is 500ppm-5000ppm, optionally 500ppm-3000ppm.

11. The battery cell according to any one of claims 1 to 10, characterized in that, The porosity of the positive electrode film layer is 14%-28%.

12. The battery cell according to any one of claims 1 to 11, characterized in that, The resistivity of the positive electrode film layer is 10 Ω·cm-35 Ω·cm.

13. The battery cell according to any one of claims 1 to 12, characterized in that, The single-side thickness of the positive electrode film layer is denoted as H, H is 70 μm-120 μm, optionally 90 μm-120 μm, and further optionally 100 μm-120 μm.

14. The battery cell according to any one of claims 1 to 13, characterized in that, A base coat layer is disposed in the bottom region of the positive electrode film layer adjacent to the positive current collector, and the base coat layer satisfies at least one of the following conditions: (1) The base coat layer comprises a conductive agent and a binder, the conductive agent comprises carbon nanotubes and conductive carbon black, and the binder comprises a vinylidene fluoride polymer; (2) The thickness of the base coat layer is 0.5 μm-5 μm.

15. The battery cell according to any one of claims 1 to 14, characterized in that, The positive electrode film layer further comprises a dispersant, and the dispersant comprises hydrogenated nitrile butadiene rubber (HNBR).

16. The battery cell according to any one of claims 1 to 15, characterized in that, Based on the mass of the positive electrode film layer, the mass content of the dispersant is 0.5%-2%.

17. The battery cell according to any one of claims 1 to 16, characterized in that, The positive electrode film layer further comprises a conductive agent, and based on the total area of the cross section of the positive electrode film layer along the thickness direction of the electrode plate, the area proportion of the agglomerated regions of the conductive agent is 0.5%-2.5%, optionally 1.5%-2.5%.

18. The battery cell according to claim 17, characterized in that, The conductive agent comprises carbon nanotubes, and the carbon nanotubes are one or more selected from single-walled carbon nanotubes, few-walled carbon nanotubes and multi-walled carbon nanotubes, optionally, the conductive agent further comprises conductive carbon black.

19. The battery cell according to claim 17 or 18, characterized in that, The agglomerated region of the conductive agent comprises carbon nanotubes and conductive carbon black.

20. The battery cell according to any one of claims 18 or 19, characterized in that, Based on the mass of the positive electrode film layer, the mass content C1 of carbon nanotubes satisfies: 0<C1≤2.5%, and the mass content C2 of conductive carbon black satisfies: 0<C2≤2.5%.

21. The battery cell according to any one of claims 1 to 20, characterized in that, The battery cell further includes a separator disposed between the positive electrode and the negative electrode. The separator includes a base film, ceramic layers disposed on both sides of the base film, and an adhesive layer disposed on at least one side of the ceramic layer away from the base film. The adhesive layer is a continuous layer with a porous structure and includes a vinylidene fluoride polymer.

22. The battery cell according to claim 21, characterized in that, The diaphragm satisfies at least one of the following conditions: (1) The thickness of the base film is 7-9 μm; (2) The thickness of the ceramic layer on one side is 2-4 μm; (3) The thickness of the adhesive layer on one side is 1-5 μm.

23. The battery cell according to any one of claims 1 to 22, characterized in that, The battery cell includes a housing, and at least one of the stacked cells is housed within the housing. The housing has a length dimension of L0, a width dimension of W0, and a thickness dimension of H0, wherein 450mm≤L0≤1300mm, 100mm≤W0≤150mm, and 14mm≤H0≤22mm.

24. The battery cell according to claim 23, characterized in that, The length dimension L0 of the shell satisfies: 450mm≤L0≤650mm.

25. The battery cell according to claim 23 or 24, characterized in that, The length dimension L0 of the shell satisfies: 900mm≤L0≤1300mm.

26. The battery cell according to claim 25, characterized in that, (1) The material of the shell is a soft-pack material, which includes an aluminum-plastic composite film, and optionally includes one or more of aluminum, polypropylene (PP), polybutylene terephthalate (PBT), polybutylene succinate (PBS), nylon, polyethylene terephthalate (PET), and polyethylene (PE); (2) The housing includes a first sealing area, which is disposed at at least one end of the laminated cell extending in the width direction; the first sealing area includes a folded edge structure extending in the length direction, and the folded edge structure is provided with encapsulating adhesive, which is continuously disposed in the length direction and fixes the folded edge structure. (3) The housing includes at least one second sealing area, which is disposed at at least one end of the laminated cell along the length direction of the housing, and the second sealing area is disposed on the tab side of the laminated cell.

27. The battery cell according to any one of claims 1 to 26, characterized in that, The outer periphery of the laminated battery cell is provided with a plurality of rubber rings that surround it along the width direction, and the rubber rings that surround it along the width direction are spaced apart along the length direction.

28. The battery cell according to any one of claims 1 to 27, characterized in that, At 25°C, the capacity of the battery cell is 105Ah-190Ah, and can be selected as 150Ah-190Ah.

29. A battery device, characterized in that, Includes the battery cell as described in any one of claims 1 to 28.

30. An electrical device, characterized in that, The electrical device includes the battery device as described in claim 29, the battery device being used to provide electrical energy.

31. An energy storage device, characterized in that, The energy storage device includes the battery device as described in claim 30, the battery device being used to store electrical energy.