New liquid-liquid phase separation microparticles (LLPS mps), and preparation method therefor and use thereof

By using LLPS technology with LLPS condensed droplets composed of PAH and Na₂S₂O₈ and Co₇-POM or Co₄-POM stabilizers, micron-sized POM-deposited particles were prepared, solving the problems of POM photocatalyst stability and recycling, enhancing photocatalytic water oxidation performance and achieving simple recycling.

WO2026236997A1PCT designated stage Publication Date: 2026-11-19INST OF CHEM
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2025/095062
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2025-05-15
Publication Date
2026-11-19

Smart Images

  • Figure CN2025095062_19112026_PF_FP_ABST
    Figure CN2025095062_19112026_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed are new LLPS MPs, and a preparation method therefor and the use thereof. The liquid-liquid phase separation (LLPS) system is composed of micron-sized liquid droplets formed under the driving by electrostatic attraction between a positively charged polyelectrolyte and a negatively charged inorganic or organic salt in an aqueous solution. A polyoxometalate (POM) is used to stabilize the system by means of electrostatic attraction, leading to the precipitation of LLPS MPs with a ridge-like structure. In the present invention, [{(B-α-PW9O34)Co3(OH)(H2O)2(O3PC(O)(C3H6NH3)PO3)}2Co]14-(Co7-POM) having photocatalytic water oxidation activity is used to induce the precipitation of microparticles, thereby making the microparticles have enhanced photocatalytic water oxidation activity and also achieving the recyclability thereof by means of simple solid-liquid separation.
Need to check novelty before this filing date? Find Prior Art

Description

A novel liquid-liquid phase separation method for micron-sized particles, its preparation method, and its application. Technical Field

[0001] This invention belongs to the field of material preparation methods, specifically relating to a novel liquid-liquid phase separation micron-sized particles, their preparation method, and their applications. Background Technology

[0002] Liquid-liquid phase separation (LLPS) originated from the study of membraneless organelles. Specifically, it refers to the phenomenon where, under certain conditions, a homogeneous solution of LLPS building blocks spontaneously separates into multiple immiscible liquid phases. Therefore, LLPS possesses unique characteristics such as dynamic reversibility, selective molecular enrichment capabilities, and microcellular compartmentalization. Through LLPS, condensed droplets with well-defined phase interfaces can spontaneously form, selectively enriching catalysts and substrates through intermolecular interactions. This increases the concentration of reactants in a confined space, thereby enhancing reaction efficiency.

[0003] Existing LLPS systems are composed of macromolecules such as peptides, surfactants, and polyelectrolytes, as well as various small molecules. Peptides include GHK, GFK, GVK, methoxy-terminated diphenylalanine (FF-OMe), polylysine, polyglutamic acid, and the cystamine conjugated derivative bis(phenylalanyl-phenylalanyl)cystamine (FFssFF), etc. Surfactants include dodecyltrimethylammonium bromide (DTAB), tetraethylammonium bromide (TAAB), sodium dodecyl sulfate (SDS), and 1,4-bis(dodecyl-N,N-dimethylammonium bromide)-2,3-butanediol (12-4(OH)2-12), etc. Polyelectrolytes include diethylaminoethyl (DEAE)-dextran, polyacrylic acid (PAA), poly(diallyldimethyl)ammonium chloride (PDDA), and poly(allylamine hydrochloride) (PAH), etc. Various small molecules include ATP, citric acid, etc.

[0004] LLPS droplets typically cannot be maintained for long periods; they will spontaneously fuse or dissolve into a homogeneous solution over time. Therefore, to maintain the stability of LLPS droplets, stabilizers need to be adsorbed onto their surface. Commonly used stabilizers include liposomes, polysaccharides, metal-organic frameworks (MOFs, often ZIF-8), and polyoxometalates (POMs) (often phosphotungstate polyanionic clusters (PTA), Ru4-POM).

[0005] Polymer oxides (POMs), as cluster compounds composed of transition metal elements (including W, Co, and V) and oxygen atoms, have attracted considerable attention due to their significant advantages in photocatalytic water oxidation, such as precise structural control, excellent oxidation stability, and outstanding multi-electron transfer capabilities. However, the inherent homogeneous solution state of POMs presents significant challenges for practical applications, particularly in terms of stability, recovery, and recyclability. A key to addressing this issue is the effective immobilization of POMs on specific supports. While some related methods have been reported, a universal and convenient approach remains lacking to achieve the homogeneous-to-heterogeneous transformation of these POM photocatalysts without sacrificing their activity. Invention Overview

[0006] This invention provides a liquid-liquid phase separation system, in which POM is used to stabilize the system and precipitate POM liquid-liquid phase separation micron-sized particles. The Co7-POM-based liquid-liquid phase separation micron-sized particles exhibit enhanced photocatalytic water splitting to produce oxygen, and can also be easily and efficiently recycled and reused. Technical issues

[0007] The main problem to be solved by this invention is how to achieve the homogeneous to heterogeneous transformation of POM photocatalysts without losing their activity. Technical solutions

[0008] To address the aforementioned problems, one objective of this invention is to provide an LLPS system.

[0009] The LLPS system provided by this invention is a micron-sized droplet formed by the electrostatic attraction between a positively charged polyelectrolyte and a negatively charged inorganic or organic salt in an aqueous solution.

[0010] The positively charged polyelectrolyte may be at least one of the following: polyallylamine hydrochloride (PAH), polydiallyldimethylammonium chloride (PDDA), polyetherimide (PEI), diethylaminoethyl dextran (DEAE-dextran), and chitosan (CHI).

[0011] The negatively charged inorganic or organic salt may be at least one of the following: Na2S2O8, sodium citrate, disodium adenosine-5'-triphosphate (ATP Na2), disodium adenosine-5'-diphosphate (ADP Na2), polyphosphate, K3[Fe(CN)6], and disodium ethylenediaminetetraacetate (EDTA-Na2).

[0012] In the LLPS system, the concentration ratio of the positively charged polyelectrolyte to the negatively charged inorganic or organic salt can be 1 mg·mL. -1 3.6 mM-1 mg·mL -1: 1000 mM, the corresponding positive and negative charge ratio can be 1: 0.67 - 1: 187.

[0013] The LLPS system provided by the present invention may further include POM, wherein the POM is used to stabilize the LLPS system.

[0014] The POM may be a POM with photocatalytic water oxidation activity;

[0015] The POM can specifically be:

[0016] .

[0017] In the LLPS system, the final concentration of POM is 0.2-2 mM.

[0018] The present invention also provides liquid-liquid phase separation micron particles (LLPS MPs) deposited by POM deposition.

[0019] The POM-deposited LLPS MPs provided by this invention have a ridge-like multilevel structure.

[0020] The POM-deposited LLPS MPs provided by this invention are prepared by a method comprising the following steps:

[0021] Add POM to the above LLPS system and stabilize for 0-48 hours (endpoint 0 is not acceptable). LLPS MPs will then precipitate spontaneously, thus obtaining the final product.

[0022] In the above method, the stabilization time can specifically be 12 hours.

[0023] The concentration of POM added to the LLPS system can be 0.2-2 mM.

[0024] The application of the above-mentioned POM-deposited LLPS MPs in photocatalytic water splitting to produce oxygen is also within the scope of protection of this invention.

[0025] In the aforementioned application, the LLPS MPs deposited by POM can specifically be LLPS MPs deposited by Co7-POM.

[0026] This invention provides a novel LLPS condensed droplet composed of PAH and Na2S2O8, which is not previously reported. Furthermore, there are no precedents for using Co7-POM or Co4-POM as stabilizers for LLPS condensed droplets. It is worth noting that previous reports often used PTA and Ru4-POM to stabilize LLPS condensed droplets, which lack photocatalytic water oxidation activity. Our reported method, however, achieves the transformation of POM from a homogeneous catalyst to a solid-phase catalyst, thus improving the photocatalytic water oxidation activity of POM and enabling its recycling.

[0027] This invention verified the deposition effects of two types of POM (Co7-POM and Co4-POM, Figures 2 and 3), both of which can rapidly prepare micron-sized particles. Among them, the micron-sized particles based on Co7-POM exhibited enhanced photocatalytic water splitting to produce oxygen, and can also be easily and efficiently recycled and reused.

[0028] Therefore, we developed a simple strategy using LLPS technology to construct POM-based LLPS MPs to achieve recycling and enhance photocatalytic water oxidation performance. Beneficial effects

[0029] This invention provides an LLPS condensed droplet composed of PAH and Na2S2O8, using Co7-POM or Co4-POM as a stabilizer to stabilize the LLPS condensed droplet, spontaneously precipitating POM-deposited LLPS MPs, realizing the transformation of POM from a homogeneous catalyst to a solid-phase catalyst, which not only improves the photocatalytic water oxidation activity of POM, but also realizes the recyclability of POM.

[0030] This invention verifies the deposition effects of two types of POM (Co7-POM and Co4-POM), both of which can rapidly prepare micron-sized particles. Among them, the micron-sized particles based on Co7-POM exhibit enhanced photocatalytic water splitting to produce oxygen, and can also be easily and efficiently recycled and reused. Attached Figure Description

[0031] Figure 1 shows (a) the LLPS phase diagram obtained in Example 1 of the present invention, (b) a typical confocal micrograph, (c) a size distribution diagram, and (d) a micrograph of droplet changes over time.

[0032] Figure 2 shows (a) a schematic diagram of the preparation process of Co7-POM micron particles in Example 2 of the present invention, (b) an LLPS condensed droplet, (c) a confocal micrograph of LLPS MPs, (d) a scanning electron micrograph, and (e) a transmission electron micrograph.

[0033] Figure 3 shows (a) a schematic diagram of the preparation process of Co4-POM micron particles in Example 3 of the present invention, (b) a confocal micrograph of LLPS MPs deposited by the prepared Co4-POM, (c, d) scanning electron micrographs and (e) transmission electron micrographs.

[0034] Figure 4(a) shows the comparison of photocatalytic water oxidation activity between Co7-POM deposited LLPS microparticles and the homogeneous solution of Co7-POM in Example 4 of the present invention, and (b) shows the verification of the recyclability of Co7-POM deposited LLPS MPs. Embodiments of the present invention

[0035] The present invention will now be described in further detail with reference to specific embodiments. The given embodiments are merely illustrative of the invention and not intended to limit its scope. The embodiments provided below can serve as a guide for further improvements by those skilled in the art and do not constitute a limitation on the invention in any way.

[0036] Unless otherwise specified, the experimental methods used in the following examples are conventional methods, performed according to the techniques or conditions described in the literature in this field or according to the product instructions. Unless otherwise specified, the materials and reagents used in the following examples are commercially available.

[0037] The raw materials used in the following examples are from:

[0038] The tris(2,2'-bipyridine)ruthenium(II) dichloride hexahydrate ([Ru(bpy)3]Cl2·6H2O) was purchased from Sigma-Aldrich, CAS No. 50525-27-4.

[0039] Ammonium bromide (NH4Br, metal-based purity 99.99%, CAS No. 12124-97-9) and alendronic acid (≥98.0%, CAS No. 66376-36-1) were supplied by Aladdin.

[0040] Polyallylamine hydrochloride (PAH, molecular weight 18000, CAS No. 71550-12-4) and disodium hydrogen phosphate heptahydrate (Na2HPO4·7H2O, 99%, CAS No. 7782-85-6) are from Innochem.

[0041] Cobalt chloride hexahydrate (CoCl2·6H2O, CAS No. 7791-13-1), cobalt nitrate hexahydrate (Co(NO3)2·6H2O, metal-based purity 99.99%, CAS No. 10026-22-9), sodium dihydrogen phosphate (NaH2PO4, 99.9%, CAS No. 7758-80-7), and sodium persulfate (Na2S2O8, metal-based purity 99.9%, CAS No. 7775-27-1) are to be purchased from Macklin Company.

[0042] Acetic acid (CH3COOH) was purchased from Concord Technologies.

[0043] Phosphoric acid (H3PO4, 85%) was produced by Beijing Chemical Plant.

[0044] Sodium hydroxide (NaOH), hydrochloric acid (HCl), sodium chloride (NaCl), and sodium tungstate dihydrate (Na2WO4·2H2O, CAS No. 20042618) were all purchased from Sinopharm Chemical Reagent Co., Ltd.

[0045] All reagents were of analytical grade and used directly without further purification. The experimental water was 18.2 MΩ·cm deionized water prepared by the ELGA PURELAB ultrapure water system in the UK.

[0046] Na9[A-α-PW9O 34 Synthesis of Na₂WO₄·2H₂O (GHPJ Domaille, A. Téazéa, Inorganic Syntheses, 27 (1990) 96-104.): 24 g (0.073 mol) of sodium tungstate dihydrate (Na₂WO₄·2H₂O) was completely dissolved in 30 mL of distilled water. The pH was adjusted to 8.9-9.0 by adding 85% phosphoric acid solution dropwise under vigorous stirring. Then, under continued vigorous stirring, 17.5 M acetic acid solution was slowly added dropwise to adjust the pH to 7.5. A large amount of white precipitate formed during the addition process; vigorous stirring continued for 1 hour. The precipitate was collected by filtration and dried under vacuum at 35 °C.

[0047] The synthesis method was improved based on the method reported in the literature (H. El Moll, A. Dolbecq, J. Marrot, G. Rousseau, M. Haouas, F. Taulelle, G. Rogez, W. Wernsdorfer, B. Keita, P. Mialane, A Stable Hybrid Bisphosphonate Polyoxometalate Single-Molecule Magnet, Chemistry - A European Journal, 18 (2012) 3845-3849.). The specific steps are as follows: alendronic acid (0.842 g, 3.38 mmol) and cobalt chloride hexahydrate (CoCl2·6H2O, 1.2 g, 5 mmol) were dissolved in 120 mL of deionized water and stirred continuously for 10 minutes to form a homogeneous solution. Then, Na9[A-α-PW9O] was slowly added. 34 ·7H₂O (4.8 g, 1.85 mmol) was added, and the pH was adjusted to 7.5 with 4 M NaOH solution. The reaction system was stirred at 80 °C for 1 hour to complete the reaction, and the purple powder was removed by filtration. Solid ammonium bromide (NH₄Br, 0.600 g, 6.13 mmol) was added to the filtrate, and the mixture was stirred at 80 °C for another 1 hour, then allowed to stand at room temperature to evaporate. After one week, a purple-red crystalline product, Co₇-POM, precipitated.

[0048] Na 10 [Co4(H2O)2(PW9O 34The synthesis of [2]·27H2O (Co4-POM) was carried out according to the method described in the literature (Q. Yin, JM Tan, C. Besson, YV Geletii, DG Musaev, AE Kuznetsov, Z. Luo, KI Hardcastle, CL Hill, A Fast Soluble Carbon-Free Molecular Water Oxidation Catalyst Based on Abundant Metals, Science, 328 (2010) 342-345.): Sodium tungstate dihydrate (Na2WO4·2H2O, 35.62 g, 0.108 mol), disodium hydrogen phosphate heptahydrate (Na2HPO4·7H2O, 3.22 g, 0.012 mol) and cobalt nitrate hexahydrate (Co(NO3)2·6H2O, 6.98 g, 0.024 mol) were dissolved in 100 mL of deionized water to form a purple precipitate. The pH was adjusted to 7.0 with 6 M hydrochloric acid, and the purple suspension was refluxed at 100 °C for 2 hours. After heating for 10 minutes, the solution color turned deep purple. After reflux, sodium chloride was added to saturate the solution, and heating was continued at 100 °C for 5 minutes, followed by filtration while hot. The purple precipitate was collected, redissolved in hot water, and heated to evaporate some of the solvent. It was then filtered again while hot, and the resulting filtrate was allowed to cool naturally at room temperature to allow crystallization. Purple needle-like crystals were obtained after one week.

[0049] Example 1: Preparation of the LLPS system

[0050] A series of concentrations of 0.5, 1, 2, 5, 10, 30, 50 and 100 mg·mL were used. -1 PAH solution was mixed with equal volumes of Na₂S₂O₈ solutions at concentrations of 1, 5, 10, 15, 25, 50, 100, 200, 350, 500, 1000, and 2000 mM. The turbidity, particle size distribution, and fusion process of the resulting mixtures were observed using a laser scanning confocal microscope (CLSM). The solubility limit of Na₂S₂O₈ in water at 20 °C is 550 g·L⁻¹. -1 (Equivalent to 2310 mM). The final confirmed formation range of LLPS is PAH (mg·mL). -1 The concentration ratio of Na2S2O8 (mM) to Na2S2O8 (mM) is 1:3.6 - 1:1000, and the corresponding positive and negative charge ratio is 1:0.67 - 1:187.

[0051] Figure 1(a) shows the phase diagram of the LLPS system, (b) shows a typical confocal micrograph, (c) shows the size distribution diagram, and (d) shows the droplet size distribution over time. The concentration of the PAH solution used to prepare the LLPS system shown in figures (b), (c), and (d) is 2 mg·mL⁻¹. -1 The concentration of the Na2S2O8 solution was 25 mM.

[0052] As shown in Figure 1, a novel type of LLPS condensed droplet was successfully formed.

[0053] Example 2: Preparation of LLPS MPs deposited by Co7-POM

[0054] 1 mL 2 mg·mL -1 Upon mixing PAH solution with 1 mL of 25 mM Na₂S₂O₈ solution, LLPS droplets immediately formed. Subsequently, after adding 1 mL of 0.9 mM Co₇-POM solution and stabilizing for 12 hours, LLPS MPs spontaneously precipitated at the bottom of the centrifuge tube. The sample was centrifuged at 2000 rpm·min⁻¹. -1 Centrifuge at a certain speed and wash with water three times to remove residual molecules.

[0055] Figure 2 shows (a) a schematic diagram of the preparation process of Co7-POM micron particles, (b) LLPS condensed droplets, (c) LLPS MPs related confocal microscopy, (d) scanning electron microscopy, and (e) transmission electron microscopy.

[0056] Example 3: Preparation of LLPS MPs deposited by Co4-POM

[0057] 1 mL 2 mg·mL -1 Upon mixing PAH solution with 1 mL of 25 mM Na₂S₂O₈ solution, LLPS droplets immediately formed. Subsequently, after adding 1 mL of 1.5 mM Co₄-POM solution and stabilizing for 12 hours, LLPS MPs spontaneously precipitated at the bottom of the centrifuge tube. The sample was centrifuged at 2000 rpm·min⁻¹. -1 Centrifuge at a certain speed and wash with water three times to remove residual molecules.

[0058] Figure 3 shows (a) a schematic diagram of the preparation process of Co4-POM microparticles, (b) a confocal micrograph of LLPS MPs, (c, d) scanning electron micrographs and (e) transmission electron micrographs.

[0059] Example 4: Determination of the photocatalytic water oxidation activity of Co7-POM deposited LLPS MPs

[0060] The operation of Example 2 was repeated to prepare multiple tubes, and the collected samples were then freeze-dried to further verify their photocatalytic water oxidation activity.

[0061] Photocatalytic water oxidation activity: Visible light-driven water oxidation was validated using a mature photosensitizer / sacrificial agent / catalyst system (YV Geletii, Z. Huang, Y. Hou, DG Musaev, T. Lian, CL Hill, Homogeneous Light-Driven Water Oxidation Catalyzed by a Tetraruthenium Complex with All Inorganic Ligands, Journal of the American Chemical Society, 131 (2009) 7522-7523.). Oxygen production was analyzed using a Clark-type oxygen electrode. A 420 nm long-pass filter (I = 40 mW·cm⁻¹) was used. -2 A 300 W xenon lamp (CEL-HXF300) simulates natural sunlight. An appropriate amount of LLPS MPs is dispersed in [Ru(bpy)3]. 2+ and S2O8 2- The mixture was placed in a solution, and then 1 mL of the mixture was transferred to the reaction chamber. After the signal stabilized, illumination was started to monitor O2 production. The reaction conditions were as follows: 1 mg / mL -1 LLPS MPs (0.07 mM Co7-POM was determined by ICP-MS), and 5 mM Na2S2O was added. 8 + LLPS MPs contain 1.4 mM Na2S2O8, 1 mM [Ru(bpy)3]Cl2, 20 mM sodium phosphate buffer (pH 8.0), V = 1 mL and T = 25 ℃.

[0062] Figure 4 shows (a) the comparison of photocatalytic water oxidation activities between Co7-POM deposited LLPS microparticles and a homogeneous Co7-POM solution, and (b) the verification of the recyclability of Co7-POM deposited LLPS MPs.

[0063] As shown in Figure 4, the LLPS MPs deposited by Co7-POM exhibit photocatalytic water oxidation activity, and their activity is higher than that of the homogeneous solution of Co7-POM. Oxygen production was analyzed using a Clark-type oxygen electrode equipped with a 420 nm long-pass filter (I = 40 mW·cm⁻¹). -2A 300 W xenon lamp (CEL-HXF300) was used to simulate natural sunlight. 1 mL of a mixed solution of the three was transferred to the reaction chamber. After the signal stabilized, illumination was started to monitor O2 production. The reaction conditions were as follows: 0.07 mM Co7-POM, 6.4 mM Na2S2O8, 1 mM [Ru(bpy)3]Cl2, 20 mM sodium phosphate buffer (pH 8.0), V = 1 mL and T = 25 ℃. The activity was higher (Figure 4(a)). The building block Na2S2O8 of LLPS can act as a sacrificial electron acceptor required for the photocatalytic water oxidation system, thereby promoting electron transfer efficiency. This type of LLPS MP with photocatalytic water oxidation function has not been reported before. It achieves both the recovery and recycling of the homogeneous catalyst POM (Figure 4(b)) and improves the photocatalytic water oxidation activity. Industrial applicability

[0064] This invention provides an LLPS condensed droplet composed of PAH and Na2S2O8, using Co7-POM or Co4-POM as a stabilizer to stabilize the LLPS condensed droplet, spontaneously precipitating POM-deposited LLPS MPs, realizing the transformation of POM from a homogeneous catalyst to a solid-phase catalyst, which not only improves the photocatalytic water oxidation activity of POM, but also realizes the recyclability of POM.

[0065] This invention verifies the deposition effects of two types of POM (Co7-POM and Co4-POM), both of which can rapidly prepare micron-sized particles. Among them, the micron-sized particles based on Co7-POM exhibit enhanced photocatalytic water splitting to produce oxygen, and can also be easily and efficiently recycled and reused.

Claims

1. An LLPS system, which is a micron-sized droplet formed by electrostatic attraction between a positively charged polyelectrolyte and a negatively charged inorganic or organic salt in an aqueous solution.

2. The LLPS system of claim 1, wherein, The positively charged polyelectrolyte is selected from at least one of the following: polyallylamine hydrochloride (PAH), polydiallyl dimethyl ammonium chloride (PDDA), polyetherimide (PEI), diethylaminoethyl dextran (DEAE-dextran), and chitosan (CHI); The negatively charged inorganic or organic salt is selected from at least one of the following: Na2S2O8, sodium citrate, disodium adenosine-5'-triphosphate (ATP Na2), disodium adenosine-5'-diphosphate (ADP Na2), polyphosphate, K3[Fe(CN)6], and disodium ethylenediaminetetraacetate (EDTA-Na2).

3. The LLPS system of claim 2, wherein, The concentration ratio of the positively charged polyelectrolyte to the negatively charged inorganic salt or organic salt in the LLPS system is 1 mg·mL -1 : 3.6 mM-1 mg·mL -1 : 1000 mM, and the corresponding positive-to-negative charge ratio is 1:0.67-1:

187.

4. The LLPS system of claim 1, wherein, The LLPS system also includes POM, which is used to stabilize the LLPS system. In the LLPS system, the final concentration of POM is 0.2-2 mM.

5. The LLPS system of claim 4, wherein, The POM is selected from: 。 6. A POM-deposited LLPS MPs, characterized in that, The POM-deposited LLPS MPs were prepared by a method comprising the following steps: Add POM to the LLPS system according to any one of claims 1-3 and stabilize for 0-48 h (endpoint 0 is not acceptable). LLPS MPs will then spontaneously precipitate, thus obtaining the desired product.

7. The POM-deposited LLPS MPs of claim 6, wherein, After adding POM, the final concentration of POM in the LLPS system is 0.2-2 mM.

8. The application of the POM-deposited LLPS MPs as described in claim 6 or 7 in the photocatalytic splitting of water to produce oxygen.