A method for shrinking a diameter of a silicon nanopore

A low-temperature wet chemical oxidation process for silicon nanopores addresses the challenges of high cost and complexity in existing methods, achieving precise diameter control and functionalization for molecular sensing and sequencing applications.

WO2026237014A1PCT designated stage Publication Date: 2026-11-19THE CHINESE UNIVERSITY OF HONG KONG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2025/095189
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2025-05-15
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing methods for manufacturing silicon nanopores face challenges with high costs, complex equipment requirements, thermal damage, and difficulty in achieving precise control and scalability, particularly for applications in molecular sensing and sequencing.

Method used

A low-temperature wet chemical oxidation process is used to grow a conformal silicon dioxide layer on the inner surface of silicon nanopores, allowing precise control over the nanopore diameter through manipulation of reaction time, temperature, and oxidizing agent concentration.

Benefits of technology

The method enables cost-effective, scalable, and precise control of nanopore dimensions, enhancing structural stability and functionalization for applications in molecular sensing, sequencing, and nanoscale electronics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2025095189_19112026_PF_FP_ABST
    Figure CN2025095189_19112026_PF_FP_ABST
Patent Text Reader

Abstract

A method for shrinking a diameter of a silicon nanopore, and a silicon nanopore produced using the method thereof. The method comprises the step of: providing a silicon substrate comprising with a nanopore having an inner surface defining an initial diameter of the nanopore; and growing a silicon dioxide layer on the inner surface of the nanopore through chemical reaction between a wet chemical oxidizing solution and the silicon substrate submerged therein for a predetermined period of time to shrink the initial diameter to a predetermined target diameter by controlling a thickness of the grown silicon dioxide layer.
Need to check novelty before this filing date? Find Prior Art

Description

A METHOD FOR SHRINKING A DIAMETER OF A SILICON NANOPORETECHNICAL FIELD

[0001] The present invention relates generally to the field of nanotechnology and nanometer-scale device fabrication, and more specifically to methods for precisely controlling the dimensions of silicon nanopores using wet chemical oxidation.BACKGROUND

[0002] Nanopores, particularly silicon-based nanopores, are structures with nanometer-scale openings that have garnered significant interest for various applications, including DNA / RNA sequencing, single-molecule sensing, filtering, and nanoscale electronics. The functionality and performance of devices incorporating nanopores often depend critically on the precise control of the nanopore diameter.

[0003] For example, silicon nanopores may be manufactured by first depositing passivation layers on both sides of a silicon sample, followed by photolithography to create square patterns. Plasma etching is then used to remove exposed passivation material, and finally, the silicon front side is etched to fabricate an inverted micro-pyramid structure. The nanopore forms at the intersection between the micro-pyramid and the truncated pyramid base.SUMMARY OF THE INVENTION

[0004] The invention provides a method for precisely shrinking the diameter of silicon nanopores utilizes wet chemical oxidation at low temperatures, i.e. 100℃ or lower. The method involves immersing a silicon nanopore in a selected oxidizing solution, such as hydrogen peroxide or Piranha solution, under controlled conditions (temperature, time, concentration) . This process grows a conformal silicon dioxide (SiO2) layer on the nanopore's inner surface, controllably reducing its diameter to a predetermined target size with nanometer precision. The resulting SiO2 layer enhances structural stability and introduces surface hydroxyl groups, facilitating functionalization of the silicon nanopore.

[0005] This cost-effective and scalable method avoids high temperatures and complex equipment, making it suitable for producing precisely sized nanopores for applications including molecular sensing, DNA / RNA sequencing, filtering, and nanoscale electronic devices.

[0006] In accordance with a first aspect of the present invention, there is provided a method for shrinking a diameter of a silicon nanopore, comprising the steps of providing a silicon substrate comprising with one or more nanopores nanopore having an inner surface defining an initial diameter of the nanopore; and growing a silicon dioxide layer on the inner surface of the nanopore through chemical reaction between a wet chemical oxidizing solution and the silicon substrate submerged therein for a predetermined period of time to shrink the initial diameter to a predetermined target diameter by controlling a thickness of the grown silicon dioxide layer.

[0007] In accordance with the first aspect, the wet chemical oxidizing solution comprises a solution of a strong oxidizing agent.

[0008] In accordance with the first aspect, the substrate comprising the silicon nanopore is immersed in a wet chemical oxidizing solution at a controlled temperature below 100℃, and does not require a high temperature process or vacuum process.

[0009] In accordance with the first aspect, at least one of a reaction time, the reaction temperature, a concentration of the wet chemical oxidizing solution, or a ratio of a compound oxidation solution is controlled or optimized.

[0010] In accordance with the first aspect, the wet chemical oxidizing solution comprises hydrogen peroxide.

[0011] In accordance with the first aspect, the wet chemical oxidizing solution comprises hydrogen peroxide of 30%concentration.

[0012] In accordance with the first aspect, the wet chemical oxidizing solution is controlled at a reaction temperature in a range of 20℃ to 70℃. for example, 20℃ to 30℃ for stronger oxidizing solution such as Piranha solution, 50℃ to 70℃ or weaker solution such as diluted hydrogen peroxide.

[0013] In accordance with the first aspect, the wet chemical oxidizing solution further comprises concentrated sulfuric acid.

[0014] In accordance with the first aspect, the wet chemical oxidizing solution comprises a Piranha solution.

[0015] In accordance with the first aspect, the volume ratio between concentrated sulfuric acid and 30 %hydrogen peroxide solution is 3: 1 to 7: 1.

[0016] In accordance with the first aspect, the wet chemical oxidizing solution may be alternatively selected from the group consisting of an ozone solution, an ammonium persulfate solution, a sodium persulfate solution, a sodium hypochlorite solution, a peroxymonosulfuric acid solution, a concentrated sulfuric acid solution, and a concentrated nitric acid solution.

[0017] In accordance with the first aspect, the silicon substrate is submerged in a corrosion-resistant bath.

[0018] In accordance with the first aspect, the method further comprises the step of agitating the wet chemical oxidizing solution in the corrosion-resistant bath during the predetermined period of time.

[0019] In accordance with the first aspect, the agitation is introduced by a thermostatic shaking hotplate.

[0020] In accordance with the first aspect, the initial diameter is in the range of 3 nm to 1000 nm.

[0021] In accordance with the first aspect, the predetermined target diameter is in the range of 1 nm to 500 nm.

[0022] In accordance with the first aspect, the grown silicon dioxide layer has a thickness in the range of 0.5 nm and 400 nm.

[0023] In accordance with the first aspect, the reaction time is controlled to be between 1 minute and 120 minutes.

[0024] In accordance with the first aspect, the shrinking rate is controlled to be between 1 nm and 3 nm per 10 minutes of reaction time.

[0025] In accordance with the first aspect, the shrinking rate is controlled to be between 5 nm and 10 nm per 5 minutes of reaction time.

[0026] In accordance with the first aspect, the inner surface of the nanopore is functionalized by a plurality of hydroxyl functional groups.

[0027] In accordance with the first aspect, the method further comprises the step of cleaning the silicon substrate comprising the nanopore with deionized water.

[0028] In accordance with the first aspect, the method further comprises the step of repeating the step of growing the silicon dioxide layer on the inner surface of the nanopore through chemical reaction between the wet chemical oxidizing solution and the silicon substrate submerged therein for an addition period of time to further shrink the predetermined target diameter of the nanopore.

[0029] In accordance with the first aspect, the method further comprises the step of measuring the diameter of the silicon nanopore after completing wet oxidation of the silicon nanopore.

[0030] In accordance with the first aspect, the measuring is performed using Transmission Electron Microscopy (TEM) , Scanning Electron Microscopy (SEM) , or electrical conductivity measurement.

[0031] In accordance with the first aspect, the method further comprises the step of repeating the steps of immersing and measuring until the predetermined target diameter is achieved.

[0032] In accordance with the first aspect, the method further comprises, prior to the immersing step, cleaning the substrate comprising the silicon nanopore, e.g. with deionized water.

[0033] In accordance with a second aspect of the present invention, there is provided a silicon nanopore produced by the method of the first aspect.

[0034] In accordance with the second aspect, the silicon nanopore has an inverted pyramid shape.BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1A is a schematic diagram showing a cross-sectional view of a silicon nanopore fabricated using the method in accordance with an embodiment of the present invention.

[0036] Figure 1B is a flow diagram showing the method for shrinking a diameter of a silicon nanopore in accordance with an embodiment of the present invention.

[0037] Figure 2 is a Scanning Electron Microscope (SEM) image showing a top view of a silicon nanopore fabrication using the method in accordance with an embodiment of the present invention.

[0038] Figure 3A is a Transmission Electron Microscope (TEM) image illustrating the progressive shrinkage of a nanopore during wet oxidation with H2O2, wherein the boundary of the initial nanopore is shown.

[0039] Figure 3B is a Transmission Electron Microscope (TEM) image illustrating the progressive shrinkage of a nanopore during wet oxidation with H2O2, wherein the nanopore in its initial state before oxidation is shown.

[0040] Figure 3C is a Transmission Electron Microscope (TEM) image illustrating the progressive shrinkage of a nanopore during wet oxidation with H2O2, wherein the nanopore after a first oxidation step is shown.

[0041] Figure 3D is a Transmission Electron Microscope (TEM) image illustrating the progressive shrinkage of a nanopore during wet oxidation with H2O2, wherein the nanopore after a second oxidation step is shown.

[0042] Figure 3E is a is a magnified view of a portion of Figure 3D, highlighting the inwardly grown silicon dioxide oxidation layer.

[0043] Figure 4A is a graph plotting the change in nanopore diameter (Size in nm) over time (Time in min) during wet oxidation using H2O2 at 60℃ for two exemplary nanopores with different initial diameters.

[0044] Figure 4B is a graph plotting the change in nanopore diameter (Size in nm) over time (Time in min) during wet oxidation using Piranha solution at room temperature for four exemplary nanopores with different initial diameters.

[0045] Figure 5A is an SEM image of a nanopore after wet oxidation treatment.

[0046] Figure 5B is a plot showing the corresponding Energy-Dispersive X-ray (EDX) spectrum taken from the area indicated in Figure 5A.

[0047] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENT

[0048] The inventors, through their trials and experiments, devised that nanopores may fabricated and modified using different processes, such as high-temperature thermal oxidation (dry oxidation) or electron beam irradiation, however these processes can suffer from drawbacks including high cost, complex equipment requirements, potential thermal damage or deformation of the nanopore structure, and difficulties in achieving precise control and scalability for mass production. For instance, dry oxidation typically requires temperatures around 900℃ and specialized furnaces, while electron beam methods often necessitate expensive equipment and are time-consuming, limiting their applicability, especially for larger pores or industrial scale-up. Therefore, there exists a need for a cost-effective, controllable, and scalable method for precisely adjusting the diameter of silicon nanopores at lower temperatures.

[0049] The present invention provides a method for precisely shrinking the diameter of silicon nanopores using a wet chemical oxidation process, addressing the need for accurate, low-cost, and scalable nanopore size control. The method enables the fine-tuning of nanopore dimensions, which is crucial for applications in molecular sensing, sequencing, and other nanotechnology fields.

[0050] With reference to Figures 1A, there is shown an example embodiment of a method 100 for shrinking a diameter of a silicon nanopore, comprising the steps of: providing a silicon substrate 104 comprising with a nanopore 102 having an inner surface 106 defining an initial diameter d1 of the nanopore 102; and growing a silicon dioxide layer 108 on the inner surface 106 of the nanopore 102 through chemical reaction between a wet chemical oxidizing solution 110 and the silicon substrate 104 submerged therein for a predetermined period of time to shrink the initial diameter d1 to a predetermined target diameter d2 by controlling a thickness of the grown silicon dioxide layer 108.

[0051] Referring specifically to Figure 1A, a schematic cross-sectional view is provided to illustrate the shrinkage of a silicon nanopore diameter from an initial diameter (d1) to a final diameter (d2) via the growth of a silicon dioxide (SiO2) layer 108 upon exposure to an oxidation solution, after the diameter shrinkage process has been completed. The shrinkage of the nanopore is caused by the expansion of solid material around the aperture / nanopore 102. Theoretically, volume (or thickness) of Si expands to around 2 times upon oxidation and becomes SiO2.

[0052] In this example embodiment, a silicon nanopore structure may be formed on a bulk silicon (Si) substrate 104, shaped into a tapered geometry characteristic of an anisotropically etched inverted pyramid. A conformal layer of silicon dioxide (SiO2) , coating the inner surface 106 of the nanopore structure. This SiO2 layer 108 defines the walls of the central nanopore channel. In this example, the dimension labeled 'd2' represents the final, reduced diameter of the nanopore 102 at its narrowest point, achieved by the controlled growth of the oxide layer 108 which consumed part of the original silicon as further described in this disclosure.

[0053] For example, an as-fabricated silicon nanopore having an initial diameter of 20 nm (d1) may be modified to become a nanopore with a final diameter of 4 nm (d2) after oxide growth.

[0054] Preferably, the method 100 generally comprises providing a substrate 104 with the silicon nanopore 102, immersing it in a specific wet chemical oxidizing solution 110 at a controlled low temperature (e.g. below 100℃) , growing a silicon dioxide (SiO2) layer 108 on the nanopore's inner surface, and controlling the process parameters (reaction time, temperature, concentration) to achieve a predetermined target diameter by controlling the SiO2 layer 108 thickness.

[0055] With reference to Figure 1B, there is provided an example fabrication process in accordance with a preferred embodiment of the present invention. In this example, an aperture (before oxidation with an initial diameter d1) is converted to a smaller aperture (after oxidation with a final diameter d2) . Figure 1B also illustrate the consumption of silicon (original boundary indicated by dashed line) and the formation of a silicon dioxide layer 108 (shaded layer as shown in the figure) resulting in the reduced diameter d2.

[0056] The starting point is a substrate 104 comprising a silicon nanopore 102 having an inner surface 106 defining an initial diameter (d1) , as illustrated schematically in Figure 1A and Figure 1B. This initial nanopore 102 can be fabricated using various known techniques, such as anisotropic etching of silicon using Potassium Hydroxide (KOH) that define a pyramid-shaped recess on one side of the Si substrate 104, followed by an isotropic etching process on the back side of the substrate 104 until the depth where the apex of the recess formed on the front side of the substrate 104 is reached. An aperture through both sides of the substrate 104 is formed then and d1 –the initial diameter of the nanopore is defined. The inventors devised that combining with techniques like the photovoltaic electrochemical etch-stop method, d1 can be controlled precisely.

[0057] Figure 2 shows a Scanning Electron Microscope (SEM) image showing a top view of an example nanopore 102 having an inverted pyramid-shaped structure formed by anisotropic etching of silicon, wherein a nanopore 102 is located at the apex of the pyramid. In this example, the nanopore 102 formed at the apex of an inverted pyramid-shaped tip may be created by anisotropic etching (e.g., using KOH) on a silicon substrate 104 mentioned above.

[0058] For example, in an experiment performed by the inventors, to generate a nanopore, initially, two 200-nm-thick Si3N4 layers were deposited on both sides of a silicon sample using plasma-enhanced chemical vapour deposition (Oxford Instruments plc) . Subsequently, two square patterns were transferred to the photoresist layers on both sides of the silicon through photolithography (SUSS MicroTec SE) , which included standard procedures such as soft baking, UV exposure, developing and hard baking. The square pattern on the front side had a side length of 30 μm, whereas that on the backside had a side length of 800 μm. Carbon tetrafluoride (flow rate: 100 sccm; gas generation time: 20 min) and argon (flow rate: 5 sccm; gas generation time: 20 min) were then introduced into a plasma chamber (Plasma Etch Inc. ) at a vacuum pressure of 100 mTorr to eliminate the exposed Si3N4 into a plasma environment excited by a radiofrequency electrostatic field (frequency: 3.0 MHz; output power: 29.6 W; radiofrequency generation time: 5 min) . Finally, an inverted micro-pyramid structure was fabricated on the front side of the silicon sample by etching it with 30% (w / w) KOH in water heated to 80.0 ℃ on a hotplate.

[0059] Preferably, the method 100 described herein is suitable for silicon nanopores regardless of the specific initial fabrication technique, as long as the substrate material is silicon, and the method is suitable for nanopore of different dimensions and / or configurations. Preferably, the initial diameter (d1) can vary widely, for example, d1 may be in the range of 3 nm to 1000 nm.

[0060] Prior to the oxidation step, it is preferable to clean the substrate 104 comprising the silicon nanopore 102. Preferably, this cleaning step may remove any organic residues or contaminants from the nanopore surface that might interfere with the uniformity of the subsequent oxidation process.

[0061] For example, standard cleaning procedure, involves rinsing the substrate 104, for example, by immersing it in deionized water for about 1 minute, followed by nitrogen gas blow drying, ensuring the surface is free from impurities and residual moisture. Other cleaning methods known in the art, such as plasma cleaning, or chemical cleaning using acids such as HF, may also be employed if significant contamination is present.

[0062] With reference to Figures 1A and 1B, the method 100 of shrinking the size of the nanopore includes a wet chemical oxidation step. Preferably, the substrate 104 with the cleaned nanopore 102 may be immersed in a wet chemical oxidizing solution 110, such as hydrogen peroxide or an oxidizing agent solution which oxidizes silicon to form silicon dioxide. Preferably, the wet chemical oxidizing solution 110 comprises a solution of a strong oxidizing agent.

[0063] During reaction, a chemical reaction occurs between the silicon inner surface 106 of the nanopore 102 and the oxidizing agent in the solution, resulting in the growth of a silicon dioxide (SiO2) layer 108 on this surface 106. This process is illustrated schematically in Figure 1A and Figure 1B, where the grown SiO2 layer 108 (shaded region) effectively narrows the pore diameter from d1 to d2.

[0064] The chemical reactions involved depend on the specific oxidizing agent used, examples of wet chemical oxidizing solution 110 include hydrogen peroxide and Piranha solution –a mixture of hydrogen peroxide and concentrated sulfuric acid. For example, with hydrogen peroxide, the chemical reaction is Si + 2H2O2 →SiO2 + 2H2O. Alternatively, with Piranha solution, the reaction involves H2SO4 acting primarily as a catalyst and dehydrating agent while H2O2 acts as the oxidant: Si + H2O2 + H2SO4 → SiO2 + H2O + H2. As Figure 1B illustrates, this process consumes some of the original silicon (boundary shown by dashed line) while forming the SiO2 layer 108, which occupies a larger volume than the consumed silicon.

[0065] Preferably, the wet oxidation process may be performed at a controlled temperature below 100℃, more preferably, maintained between 20℃ and 70℃. This low-temperature processing is a significant advantage over traditional thermal oxidation, which requires temperatures 900℃ or above. The low-temperature wet oxidation avoids potential thermal damage, stress, or deformation of the delicate nanopore structure, requires simpler and less expensive equipment (e.g., a chemical bath and hotplate instead of a high-temperature furnace) , reduces energy consumption, and is compatible with a wider range of device structures and materials.

[0066] In one preferred embodiment, the wet oxidation solution 110 comprises hydrogen peroxide (H2O2) , specifically 30%H2O2 in water can be used. The controlled temperature is preferably between 20℃ and 70℃, more preferably 60℃. H2O2 provides a relatively slow and highly controllable oxidation rate. The shrinkage rate using 30%H2O2 at 60℃ can be controlled to be between 1 nm and 3 nm per 10 minutes of reaction time.

[0067] A key aspect of the invention is the precise control over the final nanopore diameter (d2) . This may be achieved by carefully controlling the thickness of the grown SiO2 layer 108. The thickness of the SiO2 layer 108 is, in turn, controlled by manipulating one or more process parameters: the reaction time, the controlled temperature of the solution 110, and the selection (and concentration) of the oxidizing agent in the solution. The relationship between the SiO2 thickness (and thus the diameter reduction) and these parameters, particularly time, is approximately linear under given conditions (e.g. the oxidize layer is not too think which may affect diffusion of oxidizing chemical to the Si / SiO2 interface where oxidation reaction occurs) , allowing for predictable control. Preferably, the thickness of the grown silicon dioxide layer 108 can be controlled to be between 0.5 nm and 400 nm, enabling the final predetermined target diameter to be achieved, for example, within the range of 1 nm to 500 nm in accordance with preferred embodiments of the present invention.

[0068] The inventors experimented the technical effect of progressive growth of the oxide layer 108 and shrinkage of the pore diameter over multiple oxidation steps using H2O2, as illustrated by the Transmission Electron Microscope (TEM) images which show the progressive shrinkage of a nanopore 102 during wet oxidation with H2O2. In this example, the boundary of the initial nanopore is shown in Figure 3A; the nanopore in its initial state before oxidation is shown in Figure 3B; the nanopore after a first oxidation step is shown in Figure 3C; the nanopore 102 after a second oxidation step is shown in Figure 3D; and a magnified view showing an enlarged portion of Figure 3D, highlighting the inwardly grown silicon dioxide oxidation layer 108.

[0069] Total reaction time may also be a critical control parameter. For example the wet oxidation time can be controlled in the range of 1 minute to 120 minutes, depending on the chosen oxidant, temperature, concentration, and the desired amount of shrinkage.

[0070] With reference also to Figure 4A, there is shown a graph plotting the change in nanopore diameter (Size in nm) over time (Time in min) during wet oxidation using H2O2 at 60℃ for two exemplary nanopores with different initial diameters, illustrating a shrinkage rate of approximately 1-3 nm per 10 minutes.

[0071] Advantageously, slower oxidation rate is particularly advantageous for achieving very precise diameter adjustments, especially for nanopores with smaller initial diameters (e.g., < 20 nm) , minimizing the risk of over-oxidation or complete pore closure.

[0072] In another preferred embodiment, suitable for faster processing, especially for larger initial nanopores (> 20 nm) , the wet chemical oxidizing solution may be Piranha solution, which further comprises concentrated sulfuric acid. Piranha solution is a mixture of concentrated sulfuric acid (H2SO4) and hydrogen peroxide (H2O2) , which may be in a 3: 1 volume ratio (H2SO4: H2O2) . Due to the strong oxidizing power, Piranha solution may be more preferably used at or near room temperature, for example, between 20℃ and 30℃.

[0073] Preferably, Piranha solution may provide a significantly faster oxidation rate compared to H2O2 alone. In one example embodiment, with reference to Figure 4B, the shrinkage rate using Piranha solution can be controlled to be between 5 nm and 10 nm per 5 minutes of reaction time. Experimental data shows that an initial pore size of 70 nm was reduced to 39 nm after three rounds of oxidation, with each round lasting 5 minutes. In another trial experiment, a 52 nm pore was reduced to 22 nm under the same conditions, thus the average shrinkage rate is around 10 nm per round under such oxidation conditions. While efficient, care must be taken with Piranha solution, especially for smaller pores, due to the risk of over-oxidation.

[0074] Other oxidizing solutions capable of oxidizing silicon in a controlled manner at low temperatures may also be used, such as ozone solution (O3 in H2O) , ammonium persulfate ( (NH4) 2S2O8) solution, sodium persulfate (Na2S2O8) solution, sodium hypochlorite (NaClO) solution, peroxymonosulfuric acid (H2SO5 or Caro's acid) solution, concentrated sulfuric acid (H2SO4) itself under certain conditions, and concentrated nitric acid (HNO3) . The choice of oxidant may depend on the desired oxidation rate, required precision, initial pore size, and safety considerations.

[0075] To ensure the predetermined target diameter is reached accurately, the method may further comprise measuring the diameter of the silicon nanopore 102 after the wet oxidation step. This measurement can be performed using techniques such as Transmission Electron Microscopy (TEM) or Scanning Electron Microscopy (SEM) for direct visualization, or indirectly via electrical conductivity measurements through the pore. Based on the measurement, the process can be adjusted precisely.

[0076] Preferably, the method 100 further comprises the step of repeating the step of growing the silicon dioxide layer 108 on the inner surface 106 of the nanopore 102 through chemical reaction between the wet chemical oxidizing solution 110 and the silicon substrate 104 submerged therein for an addition period of time to further shrink the predetermined target diameter of the nanopore 102.

[0077] The steps of performing wet oxidation and measuring can be repeated iteratively until the predetermined target diameter is achieved. This feedback loop allows for very high precision in achieving the final target diameter. In addition, different oxidizing solution may be used in different oxidation steps such that the total processing time and precision may be achieved. For example, the wet oxidation process may be split into three repeating sections, first with only H2O2 so the final surface morphology of the oxide layer having a better quality due to slow reaction rate may be obtained, then with Piranha solution which forms the major thickness of the oxide formed due to a faster oxidation rate. Optionally, the process may finish with another step of H2O2 only oxidation step if a high-quality Si / SiO2 interface is needed.

[0078] The inventors devised that the primary consideration for nanopores in nanoscale molecular detection is the pore size. This method effectively achieves pore size reduction. While the oxidation process may have some impact on surface morphology, this has minimal effect on the detection capability of the nanopores. Additionally, the oxide layer formed through this oxidation method is highly stable, ensuring that the pore size remains consistent over time.

[0079] In one example embodiment, the wet oxidation step may be performed in a suitable container or bath. For example, a bath made of a corrosion-resistant material, such as polytetrafluoroethylene (PTFE) or quartz, may be use. Materials which are compatible with the strong oxidizing solutions are preferred. To ensure uniform oxidation and prevent localized variations in reaction rate due to concentration or temperature gradients, the method may further comprise agitating the wet chemical oxidizing solution during the wet oxidation step. This can be achieved, for example, using a thermostatic shaking hotplate which provides both temperature control and controlled agitation (e.g., reciprocating oscillation) . Standard laboratory safety precautions, including ventilation and appropriate personal protective equipment (gloves, goggles) , should be employed when handling these oxidizing solutions. In addition, transfer and handling of the nanopore substrates can be done using corrosion-resistant tools like PTFE tweezers.

[0080] The wet oxidation process results in a silicon nanopore structure, characterized by having a silicon dioxide layer 108 conformally grown on its inner surface 106. This SiO2 layer 108 defines the final, reduced diameter (d2) of the nanopore. In another experiment performed by the inventors, a nanopore 102’ was fabricated on a silicon substrate 104’ . Figure 5A shows an SEM image of a nanopore 102’a fter wet oxidation treatment; and Figure 5B shows the corresponding Energy-Dispersive X-ray (EDX) spectrum taken from the area indicated in Figure 5A. Significant peaks for Silicon (Si) and Oxygen (O) with an atomic percentage for Oxygen of approximately 40.9 At%are observed, thereby confirming the formation of a silicon oxide layer 108’ .

[0081] Compared to an oxide layer formed by high-temperature dry oxidation or electron beam irradiation, the SiO2 layer formed by this low-temperature wet oxidation method may have slightly different structural properties, such as density. For instance, the oxide from Piranha solution might be slightly less dense than that from H2O2 or dry oxidation. However, as described earlier, the oxide layer formed by this method is generally dense, stable, and provides passivation to the underlying silicon surface, enhancing the structural integrity and chemical resistance of the nanopore. The primary consideration for many nanopore applications is the precise final pore size, which this method effectively achieves.

[0082] In addition, the SiO2 layer 108 grown by this wet oxidation method also facilitate introduction of hydroxyl (-OH) groups on its surface, therefore the inner surface 106 of the nanopore 102 is functionalized by a plurality of hydroxyl functional groups. Advantageously, these surface hydroxyl groups render the SiO2 surface hydrophilic. This enhanced hydrophilicity improves wettability, which is beneficial for ion transport in sensing applications, and can help reduce non-specific adsorption of hydrophobic biomolecules (anti-fouling effect) , minimizing clogging and improving sensor stability.

[0083] Hydroxylation of silicon surfaces is achieved during wet oxidation of the silicon nanopore, as the oxidation solution directly introduces hydroxyl groups onto the surface. These –OH groups are generated simultaneously during the oxidation process, resulting in a uniform and stable distribution of hydroxyl groups on the surface. The presence of these hydroxyl groups allows further modification of the surface via silanization reactions, which may not be achievable as bare silicon is less reactive and difficult to functionalize.

[0084] Preferably, these hydroxyl groups may also serve as reactive sites for subsequent surface functionalization. Molecules can be chemically bonded to the -OH groups, for example, via silanization reactions followed by coupling to amines, carboxyls, or other functional molecules. This allows for the covalent attachment of specific probes, such as antibodies, aptamers, or other capture molecules, enabling highly sensitive and specific detection of target analytes like glucose, disease biomarkers, pathogens, DNA, or RNA. Advantageously, the ability to functionalize the surface significantly expands the applicability of the nanopores in biosensing and diagnostics. The hydration layer formed around the hydrophilic, functionalized pore can also improve the signal-to-noise ratio during single-molecule sensing by reducing unwanted interactions between the analyte and the pore wall. In addition, the -OH groups may also provide strong binding sites for functional coatings like polyethylene glycol (PEG) or silane coatings, enhancing the durability of surface modifications.

[0085] These embodiments may be advantageous in that the method as described produces precisely dimensioned silicon nanopores with functionalizable surfaces, making them suitable for a wide range of applications. Advantageously, the cost-effectiveness, controllability, low-temperature operation, and scalability of the described wet oxidation method make it significantly advantageous over other techniques, paving the way for wider adoption of nanopore technology in various applications, such as gene sequencing, biosensors, and semiconductor devices.

[0086] Advantageously, the ability to controllably shrink pores down to the nanometer or even sub-nanometer scale may be useful for at least the following applications.

[0087] In molecular sensing and sequencing, precisely sized nanopores are essential components in sensors for detecting single molecules. By tuning the pore diameter to match the size of target analytes (e.g., DNA bases, amino acids, small molecules) , high-sensitivity detection can be achieved by monitoring changes in ionic current as molecules translocate through the pore. This is particularly relevant for DNA / RNA sequencing technologies, protein analysis, and small molecule detection.

[0088] In medical diagnostics, functionalized nanopores can act as highly sensitive biosensors for early disease diagnosis by detecting specific biomarkers (e.g., cancer markers, pathogen DNA / proteins) in biological samples.

[0089] Advantageously, nanopores can also be used in devices for detecting gases at the single-molecule level, potentially measuring gas pressure, identifying species, or determining charge-to-mass ratios. In filtering and separation applications, in addition, membranes incorporating arrays of precisely sized nanopores can act as highly selective filters for separating molecules or particles based on size, useful in gas separation, water purification, or dialysis.

[0090] The method can be used to fabricate components for nanoelectronic devices, quantum dots, or energy storage devices (e.g., optimizing ion transport pathways in batteries or fuel cells by controlling pore size) . In addition, nanopores with controlled surface chemistry can serve as supports for catalysts, enhancing catalytic activity and selectivity due to high surface area and controlled environment.

[0091] It will be appreciated by persons skilled in the art that numerous variations and / or modifications may be made to the invention as shown in the specific embodiments without departing from the spirit or scope of the invention as broadly described. The present embodiments are, therefore, to be considered in all respects as illustrative and not restrictive.

[0092] Any reference to prior art contained herein is not to be taken as an admission that the information is common general knowledge, unless otherwise indicated.

Claims

1.A method for shrinking a diameter of a silicon nanopore, comprising the steps of:- providing a silicon substrate comprising with a nanopore having an inner surface defining an initial diameter of the nanopore; and- growing a silicon dioxide layer on the inner surface of the nanopore through chemical reaction between a wet chemical oxidizing solution and the silicon substrate submerged therein for a predetermined period of time to shrink the initial diameter to a predetermined target diameter by controlling a thickness of the grown silicon dioxide layer.2.The method of claim 1, wherein the wet chemical oxidizing solution comprises a solution of a strong oxidizing agent.3.The method of claim 1, wherein the wet chemical oxidizing solution comprises hydrogen peroxide.4.The method of claim 2, wherein the wet chemical oxidizing solution comprises hydrogen peroxide of 30%concentration.5.The method of claim 2, wherein the wet chemical oxidizing solution is controlled at a reaction temperature in a range of 20℃ to 70℃.6.The method of claim 4, wherein the wet chemical oxidizing solution further comprises concentrated sulfuric acid.7.The method of Claim 6, wherein the volume ratio between concentrated sulfuric acid and hydrogen peroxide is 3: 1 to 7: 1.8.The method of claim 6, the wet chemical oxidizing solution is controlled at a reaction temperature in a range of 20℃ to 30℃ when the wet chemical oxidizing solution comprises a mixture of concentrated sulfuric acid and hydrogen peroxide.9.The method of claim 1, wherein the silicon substrate is submerged in a corrosion-resistant bath.10.The method of claim 9, further comprising the step of agitating the wet chemical oxidizing solution in the corrosion-resistant bath during the predetermined period of time.11.The method of Claim 10, wherein the agitation is introduced by a thermostatic shaking hotplate.12.The method of claim 1, wherein the initial diameter is in the range of 3 nm to 1000 nm.13.The method of claim 1, wherein the predetermined target diameter is in the range of 1 nm to 500 nm.14.The method of claim 1, wherein the grown silicon dioxide layer has a thickness in the range of 0.5 nm and 400 nm.15.The method of claim 1, wherein the inner surface of the nanopore is functionalized by a plurality of hydroxyl functional groups.16.The method of claim 1, further comprising the step of cleaning the silicon substrate comprising the nanopore with deionized water.17.The method of Clam 1, further comprising the step of repeating the step of growing the silicon dioxide layer on the inner surface of the nanopore through chemical reaction between the wet chemical oxidizing solution and the silicon substrate submerged therein for an addition period of time to further shrink the predetermined target diameter of the nanopore.18.A silicon nanopore produced by the method of claim 1.19.The silicon nanopore of claim 18, wherein the predetermined target diameter is in the range of 1 nm to 500 nm.20.The silicon nanopore of claim 18, wherein the silicon nanopore has an inverted pyramid shape.