Preparation method for antibacterial biomass composite floor

By employing biomass-based material modification technology and a composite antibacterial system in antibacterial flooring, problems such as rapid degradation of antibacterial performance and imbalance between environmental protection and functionality have been solved, achieving a highly efficient and long-lasting antibacterial effect suitable for various environmental scenarios.

WO2026237101A1PCT designated stage Publication Date: 2026-11-19JIANGSU RISESUN NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2025/096823
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-14
Filing Date
2025-05-23
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing antibacterial flooring suffers from problems such as rapid degradation of antibacterial performance, insufficient long-term effectiveness, imbalance between the environmental friendliness and functionality of the substrate, contradiction between the uniformity of antibacterial agent dispersion and safety, limited environmental adaptability, and insufficient functional expansion.

Method used

Using biomass-based substrate modification technology, natural or synthetic antibacterial agents are uniformly dispersed inside the substrate or fixed on the surface. Through physical modification, chemical treatment and composite processing, antibacterial composite flooring with multi-dimensional performance optimization is formed. It includes wood and crop straw as core substrates, combined with technologies such as nano-TiO₂ photocatalytic layer, microencapsulated chitosan tea tree oil and nano-silver coating.

Benefits of technology

It achieves efficient and long-lasting antibacterial properties, while also possessing the renewable and low-carbon environmental characteristics of biomass materials, making it suitable for places with high environmental hygiene requirements, such as hospitals, schools, and homes.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

A preparation method for an antibacterial biomass composite floor, comprising the following steps: performing raw material pretreatment: processing wood chips into preliminarily processed wood powder, and processing crop straws into crop straw fragments; forming a wood base material by blending and extrusion and preparing a crop sheet material: forming a wood base material and a sheet material; and performing composite forming: coating the wood base material and the sheet material with a urea-formaldehyde resin to form a wood substrate and a sheet, then using a single wood substrate or sheet, or combining the wood substrate and the sheet in a stacked configuration to form an assembly, and finally cutting the assembly into a board blank. Renewable resources such as wood and crop straw are used as base materials, and a natural or synthetic antibacterial agent is uniformly dispersed within the base materials or fixed on the surfaces by means of physical modification, chemical treatment, composite processing, etc. thereby giving efficient and long-lasting antibacterial properties to the floor.
Need to check novelty before this filing date? Find Prior Art

Description

A method for preparing antibacterial biomass composite flooring Technical Field

[0001] This application relates to the field of antibacterial biomass flooring processing technology, such as a method for preparing antibacterial biomass composite flooring. Background Technology

[0002] Currently available antibacterial flooring technology faces four main bottlenecks:

[0003] a. Antibacterial properties decay rapidly and lack long-lasting effect.

[0004] Traditional antibacterial flooring often uses surface spraying of antibacterial agents (such as chlorine-containing organic antibacterial agents), but this method has two major drawbacks: First, it relies primarily on physical adhesion: the antibacterial agent has weak adhesion to the substrate and easily peels off after daily friction and cleaning, resulting in a 40%-60% decrease in antibacterial rate within 3 months (referencing GB / T21352-2020 standard testing). Second, it uses a single antibacterial mechanism: relying on the immediate release of metal ions such as nano-silver for sterilization, lacking a slow-release system, and unable to cope with the adaptive evolution of microorganisms over long-term use. Some strains (such as E. coli O157:H7) develop resistance by 30% after 6 months.

[0005] b. Imbalance between the environmental friendliness and functionality of the substrate

[0006] Two major contradictions exist in related technologies: insufficient functionality of natural substrates: although solid wood flooring is environmentally friendly, its antibacterial ability depends on post-spraying and it is prone to deformation due to moisture (a fluctuation of ±2% in moisture content results in 0.3mm / m of expansion and contraction); pollution problems of artificial boards: traditional wood-plastic composite flooring (WPC) uses petroleum-based resins such as polypropylene, and releases VOCs (formaldehyde release ≥1.5mg / L, exceeding the E0 standard) when the addition amount is ≥40%. In addition, the utilization rate of agricultural waste such as rice husks and straw is less than 30%, and the backward fiber modification technology leads to weak interfacial bonding (shear strength <5MPa).

[0007] c. The contradiction between uniform dispersion and safety of antibacterial agents

[0008] Nanoparticle antibacterial agents (such as nano zinc oxide with a particle size >100nm) are prone to agglomeration and formation of hot spots, leading to: local toxicity risks: when the concentration of nano silver ions is >50ppm, it significantly inhibits the survival rate of human epidermal cells (HaCaT) (inhibition rate >20%, ISO10993-5 standard); mechanical property degradation: when the amount of unmodified nanoparticles (such as TiO2) added is >2%, the static bending strength of the composite material decreases by 15%-20% (due to stress concentration at the fiber-resin interface).

[0009] d. Limited environmental adaptability and insufficient functional expandability

[0010] Traditional technologies are limited to a single antibacterial function and are significantly constrained by the environment: photocatalytic antibacterial relies on ultraviolet light: commercially available TiO2-based antibacterial flooring is only effective under ultraviolet irradiation (λ=254nm), and the sterilization efficiency drops by more than 60% under natural light; it fails in humid environments: in hospital wards, kitchens and other scenarios with relative humidity >80%, natural antibacterial agents such as chitosan are prone to moisture absorption and degradation, resulting in a sharp drop in the antibacterial rate (a decrease of 35% within 24 hours).

[0011] Therefore, it is necessary to develop a new type of antibacterial biomass flooring to meet market demand. Summary of the Invention

[0012] The following is an overview of the subject matter described in detail herein. This overview is not intended to limit the scope of the claims.

[0013] This application provides a method for preparing antibacterial biomass composite flooring. Addressing the technical bottlenecks of existing antibacterial flooring in terms of long-lasting effect, environmental friendliness, functional adaptability, and safety, this solution achieves a technological breakthrough through biomass substrate modification technology, composite antibacterial system construction, and multi-dimensional performance optimization, resulting in "substrate functionalization - antibacterial durability - application scenario-based application." Its core value lies in breaking through the traditional "end-stage antibacterial" mindset, achieving a deep integration of antibacterial function and biomass characteristics from the material design source. This provides a sustainable technical solution for addressing microbial contamination issues in the public health field, possessing significant industrial upgrading and social application value. By using renewable resources such as wood and crop straw as the core substrate, and through physical modification, chemical treatment, or composite processing, natural or synthetic antibacterial agents are uniformly dispersed within the substrate or fixed to its surface, thereby endowing the flooring with efficient and durable antibacterial properties. Its advantages lie in combining the renewability and low-carbon environmental characteristics of biomass materials with the hygienic safety of antibacterial function, making it suitable for places with high environmental hygiene requirements, such as hospitals, schools, kindergartens, and homes.

[0014] To solve the above problems, the technical solution adopted in this application is as follows:

[0015] A method for preparing antibacterial biomass composite flooring includes the following steps:

[0016] S1: Raw material pretreatment: Sieve the sawdust through 100 mesh, add silane coupling agent KH570 for treatment (coupling agent concentration 1%), soak in ethanol solution for 2 hours, and finally dry at 100℃ for 2 hours to obtain wood flour. Crush the crop straw through 80 mesh, treat it with 1.5% NaOH solution for 24 hours, and rinse with water until neutral to obtain crop straw shreds for later use.

[0017] S2: Antibacterial agent loading: Prepare a 0.08 mol / L AgNO3 solution, add wood flour or crop straw shreds and ultrasonically disperse for 40 min, then add 1 mol / L ascorbic acid solution and reduce at room temperature for 1.5 h, finally wash with water 3 times, dry the pre-processed wood flour and crop straw powder at 105℃ and grind them into powder to obtain pre-processed wood flour and crop straw powder for later use;

[0018] S3: Preparation of photocatalytic layer: 5g of nano-TiO2 was dispersed in 50g of acrylate emulsion, and 0.5g of dispersant was added. The mixture was then ultrasonically dispersed for 30min to obtain a photocatalytic coating.

[0019] S4: Wood-based panel co-extrusion: 60 parts of primary processed wood powder, 35 parts of high-density polyethylene (HDPE) and 5 parts of compatibilizer (PE-g-MAH) are pre-mixed and then extruded into wood-based material through a twin-screw extruder. The parameters of the twin-screw extruder are temperature 180-200℃ and screw speed 200rpm.

[0020] S5: Microcapsule preparation: 5g of chitosan (95% deacetylation) was dissolved in 100mL of 1% acetic acid solution, 3g of tea tree oil was added and emulsified at high speed, then 5g of gelatin was added to adjust the pH to 4.0, and 5mL of 2% glutaraldehyde was added for cross-linking for 2h. Finally, the microcapsules (particle size 10-15μm) were collected by centrifugation.

[0021] S6: Preparation of agricultural crop board: 80 parts of agricultural crop straw powder, 20 parts of polylactic acid PLA, and 5 parts of microcapsules are mixed and added to a twin-screw extruder to co-extrude the sheet. The twin-screw extruder is set with a temperature of 170-190℃ and a screw speed of 180rpm. Finally, it is hot-pressed at 120℃ with a pressure of 5MPa and a time of 15min.

[0022] S7: Composite molding: The wood substrate treated by S4 and the sheet treated by S6 are coated with urea-formaldehyde resin to form a wood substrate and a sheet board. Then, a blank is assembled by stacking a single wood substrate, a single sheet board, or a mixture of wood substrate and sheet board. The blank is composed of 3 to 5 layers in a crisscross pattern. Finally, the blank is hot-pressed at 140°C and 12MPa for 40 minutes and then cut into a board blank.

[0023] S8: Surface treatment: Apply a coating to the surface of the slab.

[0024] In one embodiment, the crop straw includes rice husks, corn stalks, wheat straw, and rice straw, wherein the crop straw is composed of a single rice husk, corn stalk, wheat straw, or rice straw, or a mixture of multiple types.

[0025] In one embodiment, the surface treatment involves spraying a bamboo vinegar solution and a chitosan composite solution, allowing it to dry naturally for 24 hours, then rolling on a water-based nano-silver coating, and finally curing it at 80°C for 3 hours.

[0026] In one embodiment, the chitosan composite solution is a mixture of 5% bamboo vinegar and 1.5% chitosan.

[0027] In one embodiment, the volume ratio of ascorbic acid solution in S2 is 1:1.

[0028] In one embodiment, the solid content of urea-formaldehyde resin in S7 is 65%, and the coating amount is 180 g / m2.

[0029] In one embodiment, the high-speed emulsification parameters are 10,000 rpm and the time is 5 min.

[0030] In one embodiment, the gelatin is a 5% aqueous solution.

[0031] In one embodiment, the microcapsule particle size is 10-15 μm.

[0032] Compared with related technologies, this application has the following advantages:

[0033] The antibacterial biomass composite flooring described in this application uses renewable resources such as wood and crop straw as its core substrate. Through physical modification, chemical treatment, or composite processing, natural or synthetic antibacterial agents are uniformly dispersed within the substrate or fixed to its surface, thereby endowing the flooring with highly efficient and long-lasting antibacterial properties. Its advantages lie in combining the renewable and low-carbon environmental characteristics of biomass materials with the hygienic safety of antibacterial functions, making it suitable for places with high environmental hygiene requirements, such as hospitals, schools, kindergartens, and homes.

[0034] After reading and understanding the detailed description, other aspects can be understood. Detailed Implementation

[0035] The technical solutions in the embodiments of this application are described clearly and completely below. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments in this application, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of this application.

[0036] Example 1

[0037] Antibacterial biomass flooring combining wood chips,

[0038] Substrate treatment: Wood chips are passed through a 100-mesh sieve → treated with silane coupling agent KH570 (1% concentration, soaked in ethanol solution for 2 hours) → dried at 100℃ for 2 hours to obtain wood flour;

[0039] Photocatalytic layer preparation: 5g of nano-TiO2 (nitrogen-doped, particle size 40nm) was dispersed in 50g of acrylate emulsion → 0.5g of dispersant (sodium hexametaphosphate) was added → ultrasonic dispersion for 30min → photocatalytic coating was obtained;

[0040] Antibacterial agent loading: Prepare a 0.08 mol / L AgNO3 solution, add wood flour and ultrasonically disperse for 40 min, then add 1 mol / L ascorbic acid solution and reduce at room temperature for 1.5 h, finally wash with water 3 times, dry the primary wood flour and crop straw powder at 105℃ and grind them into powder to obtain primary wood flour for later use;

[0041] Blending and extrusion: 60 parts of primary processed wood flour + 35 parts of high-density polyethylene (HDPE) + 5 parts of compatibilizer (PE-g-MAH) → premixing → twin-screw extruder (temperature 180-200℃, screw speed 200rpm) → extrusion molding into wood substrate;

[0042] Composite molding: Wood substrate coated with urea-formaldehyde resin (solid content 65%, glue amount 180g / m2) → assembled (3 layers cross-laminated) → hot-pressed at 140℃ and 12MPa for 40min → cut into 1200×150×12mm board blanks.

[0043] Surface treatment: Spray bamboo vinegar and chitosan composite liquid, let it dry naturally for 24 hours, then roll a water-based nano silver coating, and finally cure at 80℃ for 3 hours.

[0044] Example 2

[0045] Antibacterial biomass flooring incorporating crop straw materials,

[0046] Straw processing: Rice husks, corn stalks, wheat straw, and rice straw are crushed through an 80-mesh sieve → soaked in a 1.5% NaOH solution for 24 hours → rinsed with water until neutral to obtain crop straw fragments;

[0047] Antibacterial agent loading: Prepare a 0.08 mol / L AgNO3 solution, add crop straw shreds and ultrasonically disperse for 40 min → add 1 mol / L ascorbic acid solution (volume ratio 1:1) dropwise → reduce reaction at room temperature for 1.5 h → wash with water 3 times → dry at 105℃ → grind to obtain crop straw powder (moisture content ≤10%).

[0048] Microcapsule preparation: 5g of chitosan (95% degree of deacetylation) was dissolved in 100mL of 1% acetic acid solution → 3g of tea tree oil was added → high-speed emulsification (10000rpm, 5min) → 5g of gelatin (5% aqueous solution) was added → pH was adjusted to 4.0 → 5mL of 2% glutaraldehyde was added for cross-linking for 2h → microcapsules (particle size 10-15μm) were collected by centrifugation.

[0049] Sheet preparation: 80 parts of crop straw powder + 20 parts of polylactic acid (PLA) + 5 parts of microcapsules → blending in a twin-screw extruder (temperature 170-190℃, screw speed 180rpm) → extruding sheet → hot pressing at 120℃ (pressure 5MPa, time 15min);

[0050] Composite molding: Sheet coated with urea-formaldehyde resin (solid content 65%, coating amount 180g / m2) → assembled (5 layers cross-laminated) → hot-pressed at 140℃ and 12MPa for 40min → cut into 1200×150×12mm blanks.

[0051] Surface treatment: Spray bamboo vinegar and chitosan composite liquid, let it dry naturally for 24 hours, then roll a water-based nano silver coating, and finally cure at 80℃ for 3 hours.

[0052] Example 3

[0053] Wood substrates processed from wood chips and sheets processed from crop straw are mixed and used together. During the composite molding process, the wood substrates and sheets are mixed and assembled. Finally, the assembled blanks are hot-pressed at 140℃ and 12MPa for 40 minutes and then cut into slab blanks.

[0054] The quality testing and antibacterial performance testing of an antibacterial biomass flooring incorporating natural biomass materials described in this application.

[0055] Quantitative testing: Following ISO 22196 standards, inoculation with *Escherichia coli* (ATCC 8739) and *Staphylococcus aureus* (ATCC 6538) bacterial suspensions (concentration 10) was performed. 5 The bacterial count was measured after culturing for 24 hours (CFU / mL), and the inhibition rate was calculated (≥99%).

[0056] Durability test: The sample was placed in an artificial accelerated aging chamber (UV irradiation for 8 hours / day, humidity 70%, temperature 50℃), and the antibacterial performance was tested every 30 days. The antibacterial rate was required to be ≥90% after 6 months.

[0057] Test results: Antibacterial test: ISO22196, 24h antibacterial rate ≥99.9%

[0058] Mechanical property testing

[0059] Static bending strength: GB / T17657-2022, span 150mm, loading speed 10mm / min, requirement ≥30MPa;

[0060] Surface abrasion resistance: EN13329, using Taber abrasion tester (CS-10 wheel, 1000g load), mass loss after 1000 revolutions is ≤0.08g;

[0061] Test results: Static bending strength ≥25MPa, water absorption ≤8%.

[0062] It will be apparent to those skilled in the art that this application is not limited to the details of the exemplary embodiments described above, and that this application can be implemented in other specific forms without departing from the spirit or essential characteristics of this application. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of this application is defined by the appended claims rather than the foregoing description. Thus, it is intended that all variations falling within the meaning and scope of equivalents of the claims be included within this application.

Claims

1. A method for preparing antibacterial biomass composite flooring, comprising the following steps: S1: Raw material pretreatment: Sieve the sawdust through 100 mesh, add silane coupling agent KH570 for treatment (coupling agent concentration 1%), soak in ethanol solution for 2 hours, and finally dry at 100℃ for 2 hours to obtain wood flour. Crush the crop straw through 80 mesh, treat it with 1.5% NaOH solution for 24 hours, and rinse with water until neutral to obtain crop straw shreds for later use. S2: Antibacterial agent loading: Prepare a 0.08 mol / L AgNO3 solution, add wood flour or crop straw shreds and ultrasonically disperse for 40 min, then add 1 mol / L ascorbic acid solution and reduce at room temperature for 1.5 h, finally wash with water 3 times, dry the pre-processed wood flour and crop straw powder at 105℃ and grind them into powder to obtain pre-processed wood flour and crop straw powder for later use; S3: Preparation of photocatalytic layer: 5g of nano-TiO2 was dispersed in 50g of acrylate emulsion, and 0.5g of dispersant was added. The mixture was then ultrasonically dispersed for 30min to obtain a photocatalytic coating. S4: Wood-based panel co-extrusion: Premix 60 parts of primary processed wood powder, 35 parts of high-density polyethylene (HDPE) and 5 parts of compatibilizer (PE-g-MAH), and then extrude them into wood-based materials through a twin-screw extruder. The twin-screw extruder is set to a temperature of 180-200℃ and a screw speed of 200rpm. S5: Microcapsule preparation: 5g of chitosan (95% deacetylation) was dissolved in 100mL of 1% acetic acid solution, 3g of tea tree oil was added and emulsified at high speed, then 5g of gelatin was added to adjust the pH to 4.0, and 5mL of 2% glutaraldehyde was added for cross-linking for 2h. Finally, the microcapsules (particle size 10-15μm) were collected by centrifugation. S6: Preparation of agricultural crop board: 80 parts of agricultural crop straw powder, 20 parts of polylactic acid PLA, and 5 parts of microcapsules are mixed and added to a twin-screw extruder to co-extrude the sheet. The twin-screw extruder is set with a temperature of 170-190℃ and a screw speed of 180rpm. Finally, it is hot-pressed at 120℃ with a pressure of 5MPa and a time of 15min. S7: Composite molding: The wood substrate treated by S4 and the sheet treated by S6 are coated with urea-formaldehyde resin to form a wood substrate and a sheet board. Then, a blank is assembled by stacking a single wood substrate, a single sheet board, or a mixture of wood substrate and sheet board. The blank is composed of 3 to 5 layers in a crisscross pattern. Finally, the blank is hot-pressed at 140°C and 12MPa for 40 minutes and then cut into a board blank. S8: Surface treatment: Apply a coating to the surface of the slab.

2. The method of claim 1, wherein: The crop straw includes rice husks, corn stalks, wheat straw, and rice straw, and may be composed of a single type of rice husk, corn stalk, wheat straw, or rice straw, or a mixture of multiple types.

3. The method of claim 1, wherein: The surface treatment involves spraying bamboo vinegar and chitosan composite liquid, allowing it to dry naturally for 24 hours, then rolling on a water-based nano-silver coating, and finally curing it at 80°C for 3 hours.

4. The method of claim 3, wherein: The chitosan composite solution is a mixture of 5% bamboo vinegar and 1.5% chitosan.

5. The method of claim 1, wherein: The volume ratio of ascorbic acid solution in S2 is 1:

1.

6. The method of claim 1, wherein: The urea-formaldehyde resin in S7 has a solid content of 65% and a glue application amount of 180 g / m 2 .

7. The method of claim 1, wherein: The high-speed emulsification parameters are 10,000 rpm and the time is 5 min.

8. The method of claim 1, wherein: The gelatin is a 5% aqueous solution.