Composite laser Anti-counterfeiting packaging material and preparation method therefor
By using a new structure and simplified process for composite laser anti-counterfeiting packaging materials, the problems of long production cycles and high costs of traditional anti-counterfeiting laser packaging materials have been solved, enabling rapid response to personalized needs and cost reduction.
Patent Information
- Application Number
- PCT/CN2025/098256
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-16
- Filing Date
- 2025-05-30
- Publication Date
- 2026-11-19
AI Technical Summary
Existing anti-counterfeiting laser packaging materials have long production cycles and high costs, and cannot meet the market's rapid response to personalized demands.
It adopts a composite structure consisting of a top coating layer, an aluminum layer, a local composite coating layer, a base film layer, an adhesive layer, a base paper layer, and a back coating layer. The local composite coating layer forms a laser pattern on the base film layer, and combined with aluminum plating, the laser and silver effects are directly achieved on the base paper, simplifying the process.
It fulfills customers' personalized needs, reduces costs, shortens waiting time, improves production efficiency, and reduces subsequent printing costs.
Smart Images

Figure CN2025098256_19112026_PF_FP_ABST
Abstract
Description
A composite laser anti-counterfeiting packaging material and its preparation method Technical Field
[0001] This invention relates to the field of anti-counterfeiting packaging materials, and in particular to a composite laser anti-counterfeiting packaging material and its preparation method. Background Technology
[0002] Currently, most anti-counterfeiting laser products used in the packaging market are made of traditional, single-color paper with patterns added through printing or hot stamping. If consumers want personalized patterns on laser paper, the current method involves creating unit patterns using a photolithography machine, producing films through UV plating, then electroforming with silver, creating working nickel plates, and finally transferring them onto a base film using a laser machine, followed by aluminum spraying. Finally, these are laminated with the base paper to form packaging materials. This process undoubtedly has a long production cycle and high costs.
[0003] With the increasing demand for anti-counterfeiting packaging paper and the growing need for personalization in the market, coupled with increasingly fierce competition in the industry, there is an urgent need to improve efficiency and reduce costs through technological innovation to meet customer needs and increase corporate profits. Summary of the Invention
[0004] In view of the above-mentioned shortcomings, the present invention provides a composite laser anti-counterfeiting packaging material and its preparation method, which can meet the personalized needs of customers, greatly reduce costs, reduce customer waiting time, and improve production efficiency.
[0005] To achieve the above objectives, the embodiments of the present invention adopt the following technical solutions:
[0006] According to a first aspect of the present invention, a composite laser anti-counterfeiting packaging material is provided, comprising, from top to bottom, a top coating layer, an aluminum layer, a partially composite coating layer, a base film layer, an adhesive layer, a base paper layer, and a back coating layer, wherein the partially composite coating layer, the base film layer, and the aluminum layer together form a laser composite film having both laser effect and silver effect.
[0007] Optionally, the localized composite coating layer comprises: a two-component acrylic resin and nano-silica, wherein the nano-silica content is 1-3%, the solid content is 17-20%, the viscosity is 18-25s, and the dry weight of the coating is 0.9-1.0 g / m². 2 Thermal efficiency is 96%.
[0008] Optionally, the topcoat is made of an acrylic resin-based water-based environmentally friendly material with a solid content of 25-30%, a viscosity of 15-22s, and a topcoat weight of 3.5-4g / m². 2 After drying, the surface tension is above 38 mN / m.
[0009] Optionally, the back coating is a water-based environmentally friendly coating made of polyvinyl alcohol, with a solid content of 8%, a viscosity of 30-40s, and a back coating amount of 4-5g / m³. 2 .
[0010] Optionally, the adhesive layer is made of acrylic resin latex with a solid content of 50-55%, a viscosity of 18-35s, and an application rate of 5-7g / m³. 2 Peel strength ≥3.5N / 15mm.
[0011] Optionally, the base film layer is a PET composite base film with a thickness of 14-23 μm and a surface tension of over 50 mN / m on both sides.
[0012] Optionally, the aluminum layer has a thickness of 380–520 angstroms, and the base paper layer uses a composite backing paper of 90–400 grams.
[0013] According to a second aspect of the present invention, a method for preparing a composite laser anti-counterfeiting packaging material is provided, comprising the following steps:
[0014] S1. The local composite coating layer is locally transferred onto the base film layer using a patterned anilox roller to form a pre-coated film;
[0015] S2. Molding the pre-coated film creates a transparent laser film in the coated areas and a transparent white film in the uncoated areas.
[0016] S3. The aluminum-coated layer of the molded film is used to form a laser composite film with laser patterns and a bright silver surface on the same surface.
[0017] S4. The laser composite film is laminated to the base paper layer through an adhesive layer to form pre-printed packaging paper;
[0018] S5. Apply a back coating and a top coating to both sides of the pre-printed packaging paper to obtain the final product.
[0019] Alternatively, the patterned anilox roller has several cells to form a pattern. During the rotation of the anilox roller, the paint in the cells is transferred to the base film layer, and the remaining paint is removed by a scraper and is not transferred to the base film layer.
[0020] Optionally, when molding the pre-coated film, for positioning products, the plate spacing is controlled by a single plate, and tension coordination control is activated for positioning products. A PID algorithm is used to dynamically adjust the unwinding and rewinding tension to achieve a laser pattern positioning accuracy of ±0.1mm, with the molding roller temperature at 155–165℃. For non-positioning products, medium-pressure laser engraving is used, with the first roller temperature at 155–160℃, the second roller temperature at 160–165℃, and the pressure at 2.0–3.0 MPa. The dry coating weight of the composite coating layer is 0.9–1.0 g / m³.2 The thermal efficiency is 96%, the aluminum layer thickness is 380–520 angstroms, and the adhesive application rate is 5–7 g / m². 2 The back coating amount is 4-5 g / m². 2 The topcoat amount is 3.5–4 g / m². 2 .
[0021] Advantages of this invention: This invention can meet the personalized needs of customers, reducing the need for a series of processes from pattern design to UV lithography, UV imposition, silver spraying, electroforming, etc., which greatly reduces costs and significantly reduces customer waiting time; This invention achieves personalized laser patterns on paper, which can reduce the production of subsequent printed patterns or reduce color groups, and can also replace hot stamping patterns, thus reducing customers' printing costs to a certain extent. Attached Figure Description
[0022] To more clearly illustrate the technical solutions in the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0023] Figure 1 is a structural schematic diagram of the composite laser anti-counterfeiting packaging material of the present invention.
[0024] The names corresponding to the serial numbers in the diagram are as follows:
[0025] 1. Back coating layer; 2. Base paper layer; 3. Adhesive layer; 4. Base film layer; 5. Partial composite coating layer; 6. Aluminum layer; 7. Top coating layer. Detailed Implementation
[0026] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. In the description of the present invention, it should be noted that the terms "top," "bottom," "one side," "the other side," "front," "back," "middle part," "inner," "top," "bottom," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of the present invention.
[0027] Example 1
[0028] As shown in Figures 1 and 2, a composite laser anti-counterfeiting packaging material includes, from top to bottom, a top coating layer 7, an aluminum layer 6, a partially composite coating layer 5, a base film layer 4, an adhesive layer 3, a base paper layer 2, and a back coating layer 1. The partially composite coating layer 5, the base film layer 4, and the aluminum layer 6 together form a laser composite film that simultaneously possesses laser and silver effects. The preparation method of the composite laser anti-counterfeiting packaging material includes the following steps:
[0029] The local composite coating layer is locally transferred onto the base film layer 4 using a patterned anilox roller to form a pre-coated film. The pre-coated film is then molded, forming a transparent laser film where there is a coating and a transparent white film where there is no coating. An aluminum-coated layer 6 is applied to the molded film to form a laser composite film with a laser pattern and a silver surface on the same surface. The laser composite film is then laminated to the base paper layer 2 using an adhesive layer 3 to form pre-printed packaging paper. A back coating layer 1 and a top coating layer 7 are applied to both sides of the pre-printed packaging paper to obtain the final product.
[0030] Furthermore, the patterned anilox roller has several cells to form a pattern. During the rotation of the anilox roller, the paint in the cells is transferred to the base film layer, while the remaining paint is removed by a scraper and is not transferred to the base film layer.
[0031] In this embodiment, the back coating 1 is a water-based environmentally friendly coating made of polyvinyl alcohol, with a solid content of 8%, a viscosity of 30s to 40s, a coating cup size of 4, and a room temperature of 18℃ to 25℃. It can effectively fill the back of the paper and better balance the paper's moisture content. The back coating amount is generally 4g / m². 2 ~5g / m 2 .
[0032] In this embodiment, the base paper layer 2 can be made of various composite base papers ranging from 90 grams to 400 grams. Depending on the product type, most cigarette packs use base papers of 90 to 250 grams, which have higher requirements for VOCs, good surface smoothness, and a front surface smoothness of 300S or higher. For cigarette packs, a base paper of 250 to 400 grams is generally required, and the smoothness requirements for the cigarette pack are relatively lower.
[0033] In this embodiment, the adhesive layer 3 is generally made of acrylic resin latex with a solid content of 50% to 55%, a viscosity of 18s to 35s, a Cotton Cup 4 rating, and a room temperature of 18℃ to 25℃. It exhibits good bonding strength, i.e., strong adhesion, good leveling, and a certain degree of tackiness; the application rate is 5g / m². 2 ~7g / m 2 .
[0034] In this embodiment, the base film layer 4 is a PET composite base film with a thickness of 14U (micrometers) or more. It can be a biaxially oriented polyester film (BOPET) with a surface tension of 50mN / m or more on both sides. Generally, the material needs to be corona treated before coating.
[0035] In this embodiment, the local composite coating layer 5 uses a traditional two-component acrylic resin with a solid content of 17%–20%, a viscosity of 18s–25s, a Coating Cup 4 coating, and a dry coating weight of 0.9g / m² at room temperature. 2 ~1.0g / m 2 The thermal efficiency is 96%. This coating has good wetting and leveling properties.
[0036] In this embodiment, the aluminum layer 6 has a thickness of 380 angstroms to 520 angstroms and is tightly bonded to the local composite coating layer 5, which increases the metallic luster of the product and has moisture-proof and oxygen-proof effects.
[0037] In this embodiment, the topcoat 7 is made of an acrylic resin-based water-based environmentally friendly material with a solid content of 25%–30%, a viscosity of 15s–22s, a Coating Cup 4 rating, a room temperature of 18℃–25℃, and a topcoat weight of 3.5g / m². 2 ~4g / m 2 The surface coating 7 has good leveling and drying properties, and after drying, the surface tension is above 38mN / m, which has good adhesion to the printing substrate.
[0038] The beneficial effects of this embodiment are as follows: This invention can realize customers' personalized needs, reduce the need for a series of processes from pattern design to UV lithography, UV imposition, silver spraying, electroforming, etc., greatly reduce costs, and reduce a lot of customers' waiting time; This invention realizes personalized laser patterns on paper base, which can reduce the production of subsequent printed patterns or reduce color groups, and can also replace printed hot stamping patterns, thus reducing customers' printing costs to a certain extent.
[0039] Example 2
[0040] This embodiment provides a method for preparing a composite laser anti-counterfeiting packaging material. This composite laser anti-counterfeiting packaging material can be used to make both ordinary non-positioning anti-counterfeiting laser materials and laser positioning anti-counterfeiting materials. The preparation method of this composite laser anti-counterfeiting packaging material includes the following steps:
[0041] Step 1: Transfer the localized composite coating layer 5 onto the base film layer 4 to form a pre-coated film; specifically, this involves processing the required groove pattern on a coating roller. During the coating process, unpatterned coating is completely scraped off by a doctor blade, while patterned coating is transferred through the mesh onto the biaxially oriented polyester film (BOPET) base film material; the coating dry weight is 0.9 g / m². 2 ~1.0g / m 2 The thermal efficiency is 96%, and the coating is fully dried. If pattern positioning printing is required, the screen spacing is controlled by constant-length stretching tension during coating, with a screen spacing deviation within ±0.3mm.
[0042] Step Two: Molding the pre-coated film to form a laser film. During molding, any standard template required by the customer can be used, such as light pillars, plain surfaces, or various decorative templates, as the background pattern. Areas with coating are embossed to create the laser pattern; areas without coating will not be embossed and will remain blank. For positioning products, the template spacing is controlled by a single template. Tension coordination control is activated for positioning products, using a PID algorithm to dynamically adjust the unwinding and rewinding tension to achieve a laser pattern positioning accuracy of ±0.1mm. The molding roller temperature is 155–165℃. For non-positioning products, medium-pressure laser engraving is used, with the first roller temperature at 155–160℃, the second roller temperature at 160–165℃, and the pressure at 2.0–3.0 MPa.
[0043] Step 3: Apply aluminum layer 6 to the molded transparent laser film to form a laser composite film. The aluminum layer 6 is 380 angstroms to 520 angstroms thick. The areas with patterns are laser-etched, while the areas without patterns are silver, achieving a perfect combination of silver and laser on a single surface.
[0044] Step 4: The laser composite film is laminated to the base paper layer 2 using a wet laminator through adhesive layer 3 to form pre-printed packaging paper. The adhesive layer 3 has an adhesive application rate of 5 g / m². 2 ~7g / m 2 ;
[0045] Step 5: Apply back coating 1 and top coating 7 to both sides of the pre-printed packaging paper to obtain the final product; wherein the back coating amount of back coating 1 is 4g / m². 2 ~5g / m 2 The topcoat weight of topcoat 7 is 3.5 g / m². 2 ~4g / m 2 This packaging material, or packaging paper, can be used in a range of products including cigarette packs, medicine packs, and food packaging.
[0046] In this embodiment, the back coating 1 is a water-based environmentally friendly coating made of polyvinyl alcohol, with a solid content of 8%, a viscosity of 30s to 40s, a coating cup size of 4, and a room temperature of 18℃ to 25℃. It can effectively fill the back of the paper and better balance the paper's moisture content. The back coating amount is generally 4g / m². 2 ~5g / m 2 .
[0047] In this embodiment, the base paper layer 2 can be made of various composite base papers ranging from 90 grams to 400 grams. Depending on the product type, most cigarette packs use base papers of 90 to 250 grams, which have higher requirements for VOCs, good surface smoothness, and a front surface smoothness of 300S or higher. For cigarette packs, a base paper of 250 to 400 grams is generally required, and the smoothness requirements for the cigarette pack are relatively lower.
[0048] In this embodiment, the adhesive layer 3 is generally made of acrylic resin latex with a solid content of 50% to 55%, a viscosity of 18s to 35s, a Cotton Cup 4, and a room temperature of 18℃ to 25℃. It has good composite strength, that is, strong adhesion, good leveling, and a certain degree of tackiness.
[0049] In this embodiment, the surface tension of the biaxially oriented polyester film (BOPET) reaches more than 48mN / m on both sides. Generally, materials need to be corona treated before coating.
[0050] In this embodiment, the partial composite coating layer 5 uses a traditional two-component acrylic resin with a solid content of 17%–20%, a viscosity of 18s–25s, a Coating Cup 4, and room temperature. This coating exhibits good wetting and leveling properties.
[0051] In this embodiment, the aluminum layer 6 is tightly bonded to the local composite coating layer 5, which increases the metallic luster of the product and has moisture and oxygen barrier effects.
[0052] In this embodiment, the topcoat 7 is made of water-based environmentally friendly acrylic resin with a solid content of 25% to 30%, a viscosity of 15s to 22s, a Coating Cup 4, and a room temperature of 18℃ to 25℃. The topcoat 7 has good leveling and drying properties, and after drying, the surface tension is above 38mN / m, and it has good adhesion to the printing substrate.
[0053] The beneficial effects of this embodiment are as follows:
[0054] 1. This invention achieves personalized customer needs by using a coating and processing roller engraving pattern technology. It reduces the need for a series of processes from pattern design to UV lithography, UV imposition, silver spraying, electroforming, etc., which are costly and complicated. This technology greatly reduces costs and significantly reduces customer waiting time.
[0055] 2. By using traditional standard and decorative patterns as backgrounds for personalized designs based on customer needs, the use of traditional patterns has been elevated. Moreover, areas without patterns can be finished in silver, achieving a perfect combination of silver finish and laser patterns on a single sheet.
[0056] 3. By engraving the coating screen and controlling the tension of fixed-length stretching, not only can conventional non-positioning products be produced (through high speed and efficiency in molding), but also positioning laser products can be produced (by controlling the spacing of the screen through single-plate molding to achieve positioning laser products).
[0057] 4. This invention achieves personalized laser patterns on paper, which can reduce the production of subsequent printed patterns or reduce the number of color groups, and can also replace printed hot stamping patterns, thereby reducing the customer's printing costs to a certain extent.
[0058] Example 3: Preparation of Composite Laser Anti-counterfeiting Packaging Paper for Cigarettes:
[0059] I. Material Composition (arranged from top to bottom)
[0060] Topcoat: Made of water-based environmentally friendly acrylic resin material with a solid content of 25%, viscosity of 18S (Ford Cup 4), room temperature of 20℃, topcoat amount of 3.8g / m², and surface tension of 40mN / m after drying, ensuring good bonding with printing ink.
[0061] Aluminum layer: 450 angstroms thick, formed by vacuum aluminum plating process, giving it a metallic luster and enhancing its moisture and oxygen barrier properties.
[0062] Local composite coating layer: Two-component acrylic resin-based coating containing 2% nano silica, 18% solid content, 20s viscosity, 1.0g / m² dry coating weight, 96% thermal efficiency, used to form laser pattern areas.
[0063] Base film layer: 18U thick PET composite base film (BOPET), with a surface tension of 52mN / m on both sides (corona treated), providing a stable supporting substrate.
[0064] Adhesive layer: Acrylic resin latex, solid content 52%, viscosity 25s, application rate 6g / m², peel strength 4N / 15mm, ensuring a firm bond between the film layer and the base paper.
[0065] Base paper layer: 150g composite base paper (common specification for cigarette packs), surface smoothness of 350S or higher, low VOC content, meeting the environmental protection requirements for tobacco packaging.
[0066] Back coating: Polyvinyl alcohol water-based coating, solid content 8%, viscosity 35s, back coating amount 4.5g / m², balances paper moisture and improves printability.
[0067] II. Preparation Steps
[0068] Pre-coated film preparation: Using an anilox roller engraved with a laser pattern exclusive to the cigarette brand (the depth of the anilox roller matches the amount of paint transferred), the local composite paint layer is locally transferred onto the PET base film at a dry weight of 1.0 g / m². The paint in the unpatterned areas is removed by a scraper to form a pre-coated film.
[0069] Compression molding: For non-positioned cigarette pack products, a medium-pressure laser process is adopted: the temperature of the first roller is 158℃, the temperature of the second roller is 163℃, and the pressure is 2.5MPa. During compression molding, the patterned areas with coating form transparent laser textures due to the thermoplastic deformation of the coating, while the uncoated areas remain in a transparent white film state.
[0070] Aluminizing treatment: Vacuum aluminizing is performed on the molded film layer, with the aluminum layer thickness controlled at 450 angstroms, so that the laser texture area presents a seven-color optical effect, and the non-textured area forms a uniform silver surface, realizing the combination of laser and silver on the same plate.
[0071] Base paper lamination: Using a wet laminator, the laser composite film is laminated with 150g tobacco base paper through an adhesive layer at an application rate of 6g / m² to form pre-printed packaging paper, ensuring a peel strength ≥3.5N / 15mm.
[0072] Double-sided coating: An acrylic resin water-based coating is applied to one side of the composite film, with a dry weight of 3.8 g / m² and a surface tension of 40 mN / m after drying, meeting the requirements for subsequent printing. A polyvinyl alcohol coating is applied to the other side of the base paper, with a dry weight of 4.5 g / m², improving the paper's smoothness and moisture resistance.
[0073] Example 4: Pakistani 250g 680*551 PET laser-positioned composite paper:
[0074] Materials: 225g Hongta white cardboard, 14.3μm PET Fuwei composite base film (50mN / m after corona treatment), 1582C composite adhesive (50% solid content), 3000B back coating, #1 top coating (containing 2% nano SiO₂, 25% solid content), and Vikae 7203D coating (containing 3wt% nano SiO₂, 17% solid content).
[0075] Coating process: 160-line electro-engraved anilox roller with the pattern required for the product, dry coating amount 1.3 g / m², plate distance control 551±0.1 mm.
[0076] Molding process: Single-plate positioning molding, using 296# light column background pattern through plate, pressure 2.5MPa, plate roller temperature 160℃, plate distance control 550.5±0.1mm.
[0077] Aluminizing process: Aluminum layer thickness 30nm.
[0078] Composite process: Start fixed length stretching, plate spacing 551±0.1mm, glue application 6.5 g / m2, dry weight: 3.2 g / m2, peel strength 4.0N / 15mm, topcoat amount: 4g / m2.
[0079] Dry weight: 1 g / m2, abrasion resistance 580 times (Taber test), ethanol wiping resistance 65 times.
[0080] Effect verification:
[0081] Anti-counterfeiting features: The laser pattern exhibits dynamic color-changing under a viewing angle of 20°-70° (certified by ISO 12947-2); the accuracy deviation is as low as 0.1mm, which enhances the product's grade and makes it difficult for general enterprises to imitate, thereby improving the enterprise's competitiveness.
[0082] Economic efficiency: The overall product cost is 1.5 yuan / ㎡, which is 40% lower than the traditional process; key products do not require hot stamping and overprinting in subsequent printing, saving more than 40% of printing costs.
[0083] Durability: After 1000 hours of accelerated aging test (85℃ / 85%RH), the aluminum layer showed no oxidation or peeling.
[0084] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations, combinations, or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be determined by the scope of the claims.
Claims
1. A composite laser security packaging material, characterized in that, The film comprises, from top to bottom, a top coating layer, an aluminum layer, a partial composite coating layer, a base film layer, an adhesive layer, a base paper layer, and a back coating layer. The partial composite coating layer, the base film layer, and the aluminum layer together form a laser composite film that has both laser effect and silver effect.
2. The composite laser security packaging material according to claim 1, characterized in that, The local composite coating layer comprises: two-component acrylic resin and nano-silica, the content of the nano-silica is 1-3%, the solid content is 17-20%, the viscosity is 18-25 s, the coating dry weight is 0.9-1.0 g / m 2 , and the thermal efficiency is 96%.
3. The composite laser security packaging material according to claim 1, wherein, The top coat uses acrylic resin water-based environmental protection material, solid content 25-30%, viscosity 15-22s, top coat amount 3.5-4g / m 2 , surface tension after drying 38mN / m or above.
4. The composite laser security packaging material according to claim 1, wherein, The back coating layer is made of water-based environmental protection coating material made of polyvinyl alcohol, solid content 8%, viscosity 30-40 s, back coating amount 4-5 g / m 2 .
5. The composite laser security packaging material according to claim 1, wherein, The adhesive layer uses acrylic resin latex, solid content 50-55%, viscosity 18-35s, sizing amount 5-7g / m 2 , peel strength ≥3.5N / 15mm.
6. The composite laser security packaging material according to claim 1, wherein, The base film layer is a PET composite base film with a thickness of 14-23 μm and a surface tension of over 50 mN / m on both sides.
7. The composite laser security packaging material according to claim 1, wherein, The aluminum layer is 380–520 angstroms thick, and the base paper layer is a composite backing paper of 90–400 grams.
8. A method of preparing a composite laser security packaging material, characterized by, The preparation of the composite laser anti-counterfeiting packaging material according to any one of claims 1-7 includes the following steps: S1. The local composite coating layer is locally transferred onto the base film layer using a patterned anilox roller to form a pre-coated film; S2. Molding the pre-coated film creates a transparent laser film in the coated areas and a transparent white film in the uncoated areas. S3. The aluminum-coated layer of the molded film is used to form a laser composite film with laser patterns and a bright silver surface on the same surface. S4. The laser composite film is laminated to the base paper layer through an adhesive layer to form pre-printed packaging paper; S5. Apply a back coating and a top coating to both sides of the pre-printed packaging paper to obtain the final product.
9. The production method according to claim 8, characterized by, The patterned anilox roller has several cells to form a pattern. During the rotation of the anilox roller, the paint in the cells is transferred to the base film layer, and the remaining paint is removed by a scraper and will not be transferred to the base film layer.
10. The preparation method according to claim 8, characterized in that, When molding the pre-coated film, for positioning products, the plate spacing is controlled by a single plate, and tension coordination control is activated. A PID algorithm is used to dynamically adjust the unwinding and rewinding tension to achieve a laser pattern positioning accuracy of ±0.1mm. The molding roller temperature is 155–165℃. For non-positioning products, medium-pressure laser engraving is used, with the first roller temperature at 155–160℃, the second roller temperature at 160–165℃, and the pressure at 2.0–3.0 MPa. The dry coating weight of the composite coating layer is 0.9–1.0 g / m³. 2 The thermal efficiency is 96%, the aluminum layer thickness is 380–520 angstroms, and the adhesive application rate is 5–7 g / m². 2 The back coating amount is 4-5 g / m². 2 The topcoat amount is 3.5–4 g / m². 2 .