Precursor glass, microcrystalline glass, chemically strengthened microcrystalline glass and glass preparation method
By designing precursor glasses suitable for low-temperature crystallization and controlling the generation of impurity phases, the problem of damage to optical and mechanical properties in the production of glass-ceramics was solved, thereby improving high crystallinity and drop resistance.
Patent Information
- Application Number
- PCT/CN2025/100265
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-15
- Filing Date
- 2025-06-10
- Publication Date
- 2026-11-19
AI Technical Summary
Existing technologies struggle to effectively remove impurity phases during the production of glass-ceramics, leading to damage to optical and mechanical properties. Furthermore, the loss of crystallinity through mild heat treatment processes cannot guarantee the overall performance of glass-ceramics.
A precursor glass suitable for low-temperature crystallization is provided. Through the design of specific components and relationships, the generation of impurity phases is controlled to meet the range of δ/η values, thereby achieving low-temperature crystallization to ensure high crystallinity and performance.
Effective control of impurity phase formation under low-temperature conditions improves the optical and mechanical properties of glass-ceramics, ensuring high crystallinity and drop resistance.
Smart Images

Figure CN2025100265_19112026_PF_FP_ABST
Abstract
Description
Precursor glass, glass-ceramic, chemically strengthened glass-ceramic and glass preparation methods Technical Field
[0001] This application relates to the field of materials technology, and more particularly to the field of glass-ceramics. Specifically, this application discloses a precursor glass, a glass-ceramic, a chemically strengthened glass-ceramic, and a method for preparing the glass. Background Technology
[0002] Microcrystalline glass contains tiny crystals within it. These tiny crystals themselves possess high strength and can hinder crack propagation when the glass is impacted and cracks form. This gives microcrystalline glass superior mechanical properties compared to ordinary glass, resulting in excellent performance in drop tests. Microcrystalline glass has experienced rapid development since the beginning of this century, with its application in mobile phone cover glass seeing particularly rapid growth in recent years. Due to its high strength and drop resistance, microcrystalline glass is highly popular in the consumer electronics market.
[0003] In the production of glass-ceramics, the precursor glass typically needs to have a strong tendency to crystallize to ensure uniform crystallization throughout the glass. This leads to the formation of impurities such as lithium metasilicate and spodumene, which impair the mechanical and optical properties of glass-ceramics to varying degrees, yet are difficult to remove during actual production. These impurities can be generated during glass melting, heat treatment, and strengthening processes. The main reason is that the crystal structure of these impurities is closely related to the structure of the glass and glass-ceramics, such as high-temperature phase transformation and structural similarity, making complete elimination difficult. Currently, related technologies generally reduce the formation of impurities through relatively mild heat treatment processes (shorter heat treatment time and / or lower heat treatment temperature), i.e., sacrificing crystallinity to obtain a purer target crystalline phase. However, this does not effectively guarantee the optical and mechanical properties of the glass-ceramics.
[0004] It is important to note that the techniques described in this section are not necessarily those previously conceived or adopted. Unless otherwise specified, no technique described in this section should be assumed to be prior art simply because it is included in this section. Similarly, unless otherwise specified, the issues mentioned in this section should not be considered to be recognized in any prior art. Technical issues
[0005] This application provides a precursor glass, a glass-ceramic, a chemically strengthened glass-ceramic, and a method for preparing the glass, aiming to at least partially solve one of the problems in the related technologies. Technical solutions
[0006] The first aspect of this application provides a precursor glass suitable for low-temperature crystallization treatment, wherein the precursor glass satisfies the following relationship: δ=a*n RO +b*(nNa2O +n K2O )+c*n Li2O , η=12.5 / (0.57+4.58*i^0.55929) 0.35≤δ / η≤0.69;
[0007] Where δ represents the ionic activity of each ion in the glass, η represents the correlation index between the kinetic energy of the thermal motion of oxide molecules in the glass and the characteristic temperature point, n represents the molar percentage content of each oxide, a, b, and c are constants, i is the characteristic temperature coefficient, 1.1 < a < 1.9, 1.5 < b < 2.7, 1.1 < c < 1.6, 5.29 < i < 9.73; where RO represents alkaline earth metal oxides, a is the calculation coefficient corresponding to alkaline earth metal oxides, b is the calculation coefficient corresponding to sodium oxide and potassium oxide, and c is the calculation coefficient corresponding to lithium oxide.
[0008] Optionally, the precursor glass also satisfies the following relationship: ε=A*n SiO2 +B*n B2O3 +C*n Al2O3 +D*n P2O5 +E*n RO + F*n R2O , 21.3≤ε≤25.6;
[0009] Where ε represents the degree of atomic packing, n represents the molar percentage content of each oxide, and A, B, C, D, E, and F are constants, with A = 26.1–28.3, B = 18.3–27.3, C = 40.2–42.7, D = 56.1–63.7, E = 12.2–22.6, and F = 10.9–36.2.
[0010] Optionally, the precursor glass also satisfies the following relationship:
[0011] ε=A*n SiO2 +B*n B2O3 +C*n Al2O3 +D*n P2O5 +12.5*n MgO +14.4*n CaO +11.2*n Li2O +20.2*n Na2O +34*n K2O , where 22.1≤ε≤24.5.
[0012] Optionally, the precursor glass comprises, in molar percentage:
[0013] SiO2 content greater than or equal to 63% and less than or equal to 72%;
[0014] Al2O3 with a content greater than or equal to 1.5% and less than or equal to 6%;
[0015] Li₂O content greater than or equal to 16% and less than or equal to 26.8%;
[0016] Na₂O content greater than or equal to 0 and less than or equal to 6.5%;
[0017] K₂O concentration greater than or equal to 0 and less than or equal to 4%;
[0018] P2O5 content greater than or equal to 0.3% and less than or equal to 2.5%;
[0019] ZrO2 greater than or equal to 0 and less than or equal to 5%;
[0020] The content of RO is greater than or equal to 0 and less than or equal to 5.3%, and the RO includes at least one of CaO, MgO, ZnO and BaO;
[0021] Clarifying agent with a concentration greater than or equal to 0 and less than or equal to 1%.
[0022] Optionally, the precursor glass further comprises, in molar percentage, 0% or less than 4.8% B2O3; and / or 0% or less than 4% TiO2; and / or 0% or less than 0.5% La2O3.
[0023] Optionally, the precursor glass comprises, in molar percentage, 1.5% and 5.5% Al2O3.
[0024] Optionally, the precursor glass comprises, by mole percentage, 2% and 4.2% Al2O3; or 3.5% and 5.2% Al2O3.
[0025] Optionally, the precursor glass comprises, by mole percentage, 0% and 2.2% P2O5.
[0026] Optionally, the precursor glass comprises, in molar percentage, 18% and 26.8% Li2O, 0% and 6.5% Na2O, and 0% and 4% K2O.
[0027] Optionally, the precursor glass comprises, in molar percentage, 22.2% and 25.8% Li2O, 0% and 3.1% Na2O, and 0% and 1.2% K2O.
[0028] Optionally, the precursor glass comprises, in molar percentage, 16% and 24% Li2O, 0% and 5% Na2O, and 0% and 4% K2O.
[0029] Optionally, the precursor glass comprises, in molar percentage, 20.5% and 23.5% Li2O, 0% and 2% Na2O, and 0% and 0.5% K2O.
[0030] Optionally, the precursor glass may further include at least one of Y2O3, La2O3, Nb2O5, Ta2O5, HfO2, and Bi2O3.
[0031] Optionally, the precursor glass, in molar percentage, satisfies at least one of the following relationships: 4 ≤ n Li2O / (n Na2O +n K2O )≤17; 6≤n Li2O / (n CaO +n MgO +n ZnO 0.24≤n ≤ 18; Li2O / (n SiO2 +n Al2O3 )≤0.38;
[0032] Li₂O, Na₂O, and K₂O are all alkali metal oxides. By adding these oxides in combination, a mixed alkali effect can be formed, improving the cross-linking density and chemical stability of the glass network, significantly enhancing the stability of glass-ceramic products. The Li₂O / (Na₂O+K₂O) ratio needs to meet certain ranges; if the (Na₂O+K₂O) ratio is too low, the mixed alkali effect cannot be formed, while if the (Na₂O+K₂O) ratio is too high, it will affect the formation ratio and rate of lithium crystals within the glass. (CaO+MgO+ZnO) has a high electric field strength. The proportion of (CaO+MgO+ZnO) can enhance the mechanical properties of glass, such as its elastic modulus and Vickers hardness. If the proportion of (CaO+MgO+ZnO) is too low, it will not achieve the beneficial effect of enhancing mechanical properties. If it is too high, it will promote the malignant growth of crystals and make it difficult to form microcrystals. (SiO2+Al2O3) is the main network forming body in glass and plays a decisive role in the viscosity and network crosslinking density of glass. If the proportion of (SiO2+Al2O3) is too low, it will not be possible to form controllable crystallization under suitable viscosity and temperature conditions. If the proportion is too high, it will affect the crystallinity and crystal size of glass, and at the same time make the glass viscosity too high, which is not conducive to production.
[0033] The second aspect of this application provides a microcrystalline glass, which is obtained by heat treatment based on the precursor glass described in the first aspect above.
[0034] Optionally, the lower crystallization temperature of the microcrystalline glass is 553–639°C, and the upper crystallization temperature is 989–1123°C.
[0035] Optionally, the microcrystalline glass has a lithium disilicate crystal phase, and the lithium disilicate crystal phase meets the following indicators: average grain size less than or equal to 38-45.7 nm, and crystallinity greater than or equal to 56.38%.
[0036] Optionally, the lithium disilicate crystal phase meets the following indicators: the size of 98% of the crystal phase is less than or equal to 60 nm, the size of 95% of the crystal phase is less than or equal to 55 nm, the size of 80% of the crystal phase is less than or equal to 50 nm, and the crystallinity is greater than or equal to 61.22%.
[0037] Optionally, the microcrystalline glass meets at least one of the following performance indicators: Vickers hardness greater than or equal to 727 kgf / mm². 2 Fracture toughness greater than or equal to 1.01 MPa·m 1 / 2 The properties are: Young's modulus greater than or equal to 99 GPa, shear modulus greater than or equal to 40 GPa, |B| value less than or equal to 0.74% at a thickness of 0.55 mm, haze less than or equal to 0.14%, and transmittance of visible light with a wavelength of 550 nm greater than or equal to 91%.
[0038] The third aspect of this application provides a chemically strengthened microcrystalline glass, which is obtained by sequentially subjecting the precursor glass of the first aspect to heat treatment and ion exchange treatment.
[0039] Optionally, the chemically strengthened glass-ceramic satisfies at least one of the following performance indicators: Vickers hardness greater than or equal to 655 kgf / mm². 2 Fracture toughness greater than or equal to 1.2 MPa·m 1 / 2 The following parameters are specified: Young's modulus greater than or equal to 98.38 GPa; shear modulus greater than or equal to 39.35 GPa; |B| value less than or equal to 0.74% at a thickness of 0.55 mm; haze less than or equal to 0.13%; transmittance relative to visible light at a wavelength of 550 nm greater than or equal to 91%; nine-point drop test height based on 32g steel ball at a thickness of 0.55 mm with a thickness of 980–1290 mm; maximum bending strength of 1052–1200 MPa; whole-machine drop test height based on 80-grit sandpaper with a thickness of 850–1020 mm; and whole-machine drop test height based on 180-grit sandpaper with a thickness of 1200–1600 mm.
[0040] The fourth aspect of this application provides a method for preparing glass, comprising:
[0041] After the raw materials are mixed evenly according to the glass formula, they are melted according to the preset melting temperature and melting time, and then annealed to obtain the precursor glass.
[0042] The precursor glass is heat-treated to obtain glass-ceramic.
[0043] The precursor glass satisfies the following relationship: δ=a*n RO +b*(n Na2O +n K2O )+c*n Li2O ), η=12.5 / (0.57+4.58*i^0.55929), 0.35≤δ / η≤0.69;
[0044] Where δ represents the ionic activity of each ion in the glass, η represents the correlation index between the kinetic energy of the thermal motion of oxide molecules in the glass and the characteristic temperature point, n represents the molar percentage content of each oxide, a, b, and c are constants, and i is the characteristic temperature coefficient, which is specifically stated in the specification: 1.1 < a < 1.9, 1.5 < b < 2.7, 1.1 < c < 1.6, 5.29 < i < 9.73.
[0045] Optionally, the heat treatment of the precursor glass includes: placing the precursor glass in a crystallization furnace, heating it to 500-610°C at a heating rate greater than or equal to 6°C / min and holding it at that temperature for 200-300 min, then heating it to 655-800°C at a heating rate greater than or equal to 6°C / min and holding it at that temperature for 60-120 min, and finally cooling it at a cooling rate less than or equal to 2°C / min.
[0046] Optionally, the heat treatment of the precursor glass includes: placing the precursor glass in a crystallization furnace, heating it to 560-590°C at a heating rate of 8-12°C / min and holding it at that temperature for 220-250 min, then heating it to 750-790°C at a heating rate of 8-12°C / min and holding it at that temperature for 70-90 min, and finally cooling it at a cooling rate of less than or equal to 2°C / min.
[0047] Optionally, the glass preparation method further includes: hot bending the microcrystalline glass through a hot bending workstation; wherein the pressure of the hot bending workstation is 0.7 to 1.1 MPa, and the running time of a single workstation is 70 to 110 s.
[0048] Optionally, the hot bending process requires four preheating stations, three hot pressing stations, and two cooling stations; wherein the operating temperature of the first preheating station is 430–470°C, the operating temperature of the second preheating station is 530–570°C, the operating temperature of the third preheating station is 630–670°C, the operating temperature of the fourth preheating station is 710–730°C, the operating temperature of the first hot pressing station is 740–760°C, the operating temperature of the second hot pressing station is 740–760°C, the operating temperature of the third hot pressing station is 580–620°C, the operating temperature of the first cooling station is 430–470°C, and the operating temperature of the second cooling station is 280–320°C.
[0049] Optionally, the glass preparation method further includes: immersing the microcrystalline glass in a chemically strengthened salt bath for ion exchange treatment to obtain chemically strengthened microcrystalline glass; wherein the chemically strengthened salt bath comprises, by mass percentage: greater than or equal to 9.99% and less than or equal to 39.99% KNO3, greater than or equal to 59.99% and less than or equal to 89.99% NaNO3, and greater than or equal to 0.03% and less than or equal to 0.1% LiNO3.
[0050] Optionally, the temperature of the chemically enhanced salt bath is 460–490°C, and the duration of the ion exchange treatment is 4–10 hours.
[0051] As can be seen from the above, the precursor glass, glass-ceramic, chemically strengthened glass-ceramic, and glass preparation method provided in this application satisfy the following relationship: δ=a*n RO +b*(n Na2O +n K2O )+c*n Li2O ), 0.35≤δ / η≤0.69; δ represents the ionic activity of each ion in the glass, η represents the correlation index between the kinetic energy of the thermal motion of oxide molecules in the glass and the characteristic temperature point, n represents the molar percentage content of each oxide, a, b, c are constants, i is the characteristic temperature coefficient, 1.1<a<1.9, 1.5<b<2.7, 1.1<c<1.6, 5.29<i<9.73; Since alkali metals and alkaline earth metals have a significant effect on increasing the crystallization tendency of glass, Na2O and K2O have a particularly prominent effect on increasing the crystallization tendency of glass. This is because their ionic radii are small and they are more easily attracted by high field strength ions under suitable temperature conditions. By introducing the δ calculation formula, oxides with different effects in the glass can be classified and calculated. By comprehensively evaluating the different factors affecting the crystallization tendency, the relationship between the electric field strength and ion migration of different oxides in the glass can be described. Then, by introducing the η calculation formula, the relationship between the kinetic energy of the thermal motion of glass oxide molecules and the characteristic temperature point is linked to the above-mentioned crystallization intensity, so as to comprehensively evaluate the crystallization tendency at lower temperatures.
[0052] Furthermore, the ionic activity of the glass is described by δ / η to characterize its crystallization tendency. Setting the value of δ / η within a specific range ensures that the glass viscosity is suitable for low-temperature crystallization. It is worth noting that "suitable for low-temperature crystallization" in this embodiment refers to a crystallization temperature lower than the thermoforming and hot-working temperatures, while still maintaining high crystallinity. Due to the relatively low crystallization temperature, the formation of impurity phases can be effectively controlled. This application optimizes the value range to ensure that the glass viscosity is suitable for low-temperature crystallization, balancing impurity phase control and the crystallinity of the target crystalline phase, thereby improving the optical and mechanical properties of the glass. It should be understood that the content described in this section is not intended to identify key or important features of this application, nor is it intended to limit the scope of this application. Further effects of the aforementioned non-conventional alternative methods will be explained below in conjunction with specific embodiments. Attached Figure Description
[0053] The accompanying drawings exemplify embodiments and form part of the specification, working together with the textual description to explain exemplary implementations of the embodiments. The drawings shown are for illustrative purposes only and do not limit the scope of the claims. Throughout the drawings, the same reference numerals refer to similar but not necessarily identical elements.
[0054] Figure 1 is a DSC test curve of the microcrystalline glass corresponding to Example 4 provided in this application;
[0055] Figure 2 is an XRD test curve of the microcrystalline glass corresponding to Example 4 provided in this application;
[0056] Figure 3 is a scanning electron microscope image of the microcrystalline glass corresponding to Example 4 provided in this application;
[0057] Figure 4 is a viscosity-temperature curve of the microcrystalline glass corresponding to Example 4 provided in this application. Embodiments of the present invention
[0058] To make the inventive objectives, features, and advantages of this application more apparent and understandable, the technical solutions in the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of this application, and not all of them. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.
[0059] In the description of the embodiments of this application, the term "multiple" means two or more, unless otherwise explicitly specified; the term "comprising" indicates the presence of the described feature, whole, step, operation, element and / or component, but does not exclude the presence or addition of one or more other features, wholes, steps, operations, elements, components and / or sets thereof; the term "and / or" describes the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can include three cases: A alone, A and B simultaneously, and B alone. The character " / " generally indicates that the related objects before and after are in an "or" relationship; the term "about" means that the content, size, parameter, etc. are not and do not need to be precise. Where necessary, they can be approximate or higher or lower. Generally speaking, regardless of whether it is explicitly stated, the content, size, parameter, etc. should be "about" or "approximate"; the terms "preferred" and "optional" are not used to limit the scope of this application, nor do they indicate that certain technical features are critical or indispensable to the implementation of this application, but should be understood as merely indicating specific aspects of the embodiments of this application.
[0060] Unless specifically indicated in the specific circumstances, the numerical ranges described in the embodiments of this application are intended to include the endpoints of the numerical ranges as well as all integers and fractions within the range. When a quantity, solubility, or other parameter is described in the form of a preferred range or preferred value, it should be understood that this is equivalent to disclosing any range by combining any preferred range with a preferred range, a preferred value with a preferred value, or a preferred range with a preferred value, without regard to whether such pairwise combinations are specifically interpreted in the embodiments.
[0061] Unless otherwise specified in the specific circumstances, the component content described in the embodiments of this application is expressed as mole percentage (mol%).
[0062] Terminology Explanation
[0063] Precursor glass: refers to glass that has not undergone nucleation, crystallization, or strengthening treatments.
[0064] Glass-ceramics, also known as glass-ceramics, are a type of solid composite material containing both a glassy phase and a microcrystalline phase, prepared through targeted and controlled heat treatment of a precursor glass. The microcrystalline phase is also referred to as the crystalline phase, crystallized phase, or crystalline phase in other sources.
[0065] Chemically strengthened glass-ceramics: refers to solid composite materials obtained by chemically strengthening glass-ceramics. It should be understood that during high-temperature chemical strengthening or high-temperature ion exchange processes, alkali metal ions with larger ionic radii (such as potassium and sodium ions) in the salt bath or molten salt will replace alkali metal ions with smaller ionic radii (such as sodium and lithium ions) in the glass-ceramics. This creates a volume difference in the exchanged ions, generating compressive stress from the surface to the interior of the glass-ceramics, which hinders and delays the propagation of microcracks, thereby improving the mechanical strength of the glass-ceramics.
[0066] Nucleation temperature: refers to the temperature at which crystal nuclei form.
[0067] Crystallization temperature: refers to the temperature at which the growth rate of the target crystal can be controlled.
[0068] Transmittance: When light of a certain wavelength shines on a glass surface, the light will be reflected, absorbed, and transmitted. The ratio of the intensity of the transmitted portion to the intensity of the incident light is the transmittance.
[0069] In this invention, the average transmittance of the glass-ceramic in the visible light range refers to the average transmittance of the glass-ceramic measured under wavelengths of 360 nm to 740 nm. This invention uses a Konica Minolta CM-3600A spectrophotometer to test the average transmittance of the glass-ceramic under wavelengths of 360 nm to 740 nm.
[0070] Crystallinity: refers to the percentage of the total mass of crystalline phases / crystals in a glass-ceramic glass.
[0071] Haze (C) refers to the percentage of transmitted light intensity that deviates from the incident light by more than 2.5° from the total transmitted light intensity. In this invention, the haze value is measured using a Konica Minolta CM-3600A spectrophotometer under a standard C light source.
[0072] L-value: In this invention, L-value is the specular reflection (SCI) L-value, which represents the brightness of the material. A positive L-value indicates a whiter appearance, and a negative L-value indicates a darker appearance.
[0073] a-value: In this invention, a-value is the specular reflection (SCI) a-value, which represents the red-green value of the material. A positive a-value indicates that the material is reddish, and a negative a-value indicates that the material is greenish.
[0074] b-value: In this invention, b-value is the specular reflection (SCI) b-value, which represents the yellow-blue value of the material. A positive b-value indicates that the material is yellowish, and a negative b-value indicates that the material is bluish.
[0075] In this invention, Vickers hardness refers to a standard for expressing the hardness of materials, proposed by Robert L. Smith and George E. Sandland in 1921 at Vickers Ltd.
[0076] In this invention, fracture toughness refers to the impedance value exhibited by a material when a crack or crack-like defect occurs in a specimen or component, and the material no longer fractures rapidly with increasing load, i.e., when an unstable fracture occurs.
[0077] In this invention, CS_50 refers to the compressive stress value at a depth of 50 μm measured from the glass surface.
[0078] In this invention, |CT_CV| refers to the absolute value of the maximum value of the tensile stress, specifically the absolute value of the maximum value among all tensile stresses in the tensile stress layer.
[0079] In this invention, |CT_AV| refers to the absolute value of the average tensile stress in the tensile stress layer, specifically the absolute value of the average value of all tensile stresses in the tensile stress layer.
[0080] In this invention, DOL_0 refers to the compressive stress layer depth, also known as the compressive stress layer depth, which is the distance from any surface of the glass to a position close to that surface where the compressive stress is zero.
[0081] In a first aspect, the present invention provides a reinforced microcrystalline glass with the following crystallization characteristics and stress characteristics in order to enable the reinforced microcrystalline glass to have excellent drop resistance.
[0082] Typical drop impacts result in piercing damage. Sharp particles easily penetrate the glass surface (CS) upon impact, creating a pit 30-50 micrometers deep. Cracks then form and propagate at this pit, breaking through the compressive stress zone and causing the glass to shatter. CS_50 represents the compressive stress at a depth of 50 micrometers. Higher stress at this depth helps inhibit crack formation at the pit. A deeper DOL-0 indicates a larger area hindering crack propagation. CT-CV represents the highest point of tensile stress, similar to the average tensile stress in CT-AV, indirectly indicating the magnitude of deep compressive stress. Better stress performance makes crack propagation more difficult.
[0083] Drop test: A glass plate was attached to a counterweight steel plate to simulate a drop of the entire machine. The counterweight steel plate weighed 200g.
[0084] The aforementioned substrate glass is heat-treated in an electric resistance furnace. The heat treatment process (nucleation temperature / nucleation time, crystallization temperature / nucleation time, and heating rate during heat treatment) yields a chemically strengthened microcrystalline glass sample brick. The microcrystalline glass sample brick is then cut, CNC machined (using a computer numerical control (CNC) machine tool; the CNC instrument used in this invention is an RCG500S), and polished to obtain a mirror-smooth microcrystalline glass sheet.
[0085] The physical properties of the prepared glass-ceramics were tested according to the following method:
[0086] Upper and lower limits of crystallization: The test was conducted using an Orton GTF-MD-16 gradient furnace. The glass strip was placed on the ceramic tube of the Orton gradient furnace, the heating parameters were set, and after the furnace cooled down, the sample was taken out and the corresponding position was recorded. Since the temperature of one end of the sample is low and the temperature of the other end is high, the temperature can be accurately determined. Refer to the standard ASTM E 228-17.
[0087] Vickers hardness test: A diamond Vickers indenter is pressed into the surface of the sample with a load of 1.916N to 49.03N to form an indentation. The load is divided by the surface area of the indentation calculated based on the average length of the diagonal of the indentation. Refer to standard GBT 37900-2019.
[0088] Fracture toughness test: A diamond Vickers indenter is pressed into the surface of the specimen to form an indentation with a load of 1.916N to 49.03N, and pre-cracks are generated at the four vertices of the indentation. The values are calculated based on the load and the indentation crack propagation length, referring to standard GBT 37900-2019.
[0089] Young's modulus testing: The Young's modulus of the sample was obtained by acoustic testing using a UMS-100 ultrasonic material characterization system, in accordance with the standard GB / T 37780-2019.
[0090] XRD Testing: Microcrystalline glass slides were ground into fine glass powder with a particle size less than 75 μm using a pulverizer. The powder was then analyzed using an X-ray diffractometer (Shimadzu XRD-6100) to obtain the XRD diffraction peak curve. The X-ray diffractometer used in this invention was a Shimadzu XRD-6100, the target material was copper, the incident angle range was 2θ = 10-80°, the scanning speed was 0.2° / min, the operating voltage was 40 kV, and the operating current was 30 mA. The crystal phase of the sample was then obtained by analyzing the XRD diffraction data using JADE software.
[0091] Average grain size: Using the XRD test results, the average grain size of the sample can be calculated according to the Scherrer formula D=Kλ / (βcosθ), where λ is the X-ray wavelength (0.154056nm), β is the full width at half maximum (FWHM) of the diffraction peak, and θ is the Bragg diffraction angle. Specifically, the RAW file (diffraction pattern) output by the XRD instrument is curve-fitted in Jade software. Jade outputs a fitting report. Based on the angle 2θ value and Peak FWHM value (FWHM of the diffraction peak) corresponding to each diffraction peak in the fitting report, and converting the Peak FWHM value to radians β=(FWHM / 180*3.14), the grain size of each diffraction peak is calculated using D=Kλ / (βcosθ), and then averaged to obtain the average grain size. Test method for crystal content / crystallinity: Import the X-ray diffraction test result file (RAW format) into the X-ray diffraction data Rietveld refinement software (such as Gsas, Fullprof, Maud, Topas), perform fitting and calculation, and the crystal content / crystallinity in the glass-ceramic sample can be obtained. The ratio of the fitted crystal phase peak area to the fitted total peak area is the crystal content, which is also referred to as crystallinity in this invention.
[0092] b-value determination: The b-value of the sample was obtained by testing the sample using a Konica Minolta CM-3600A spectrophotometer from Japan. The average value of 5 parallel samples was taken as the b-value result of the sample to be tested.
[0093] Transmittance determination: The test was conducted according to the standard GB / T 7962.12-2010 "Test Methods for Colorless Optical Glass - Part 12: Spectral Internal Transmittance". First, the microcrystalline glass sample to be tested was cleaned in an ultrasonic cleaner under the following conditions: cleaning time 5-10 min; cleaning agent: commonly used detergent diluted 10 times; cleaning temperature: 45℃-65℃; cleaning frequency: 20kHz-40kHz. Then, the transmittance under different wavelengths of light was measured using a haze meter (Konica Minolta CM-3600A spectrophotometer).
[0094] The transmittance of the sample under 550nm wavelength light was measured using a Konica Minolta CM-3600A spectrophotometer. The average value of five parallel samples was taken as the transmittance result of the sample under 550nm wavelength light.
[0095] Glass thickness: determined by micrometer measurement. It should be understood that the degree of ion exchange varies gradient from the surface to the center along the thickness direction. The total Na-K and / or Li-Na exchange amount generally does not exceed 1% of the total sample mass, and the differences in ion radii are all on the order of micrometers (pm). Therefore, the expansion effect in the thickness direction is very slight, and the thickness can be approximated as essentially unchanged. That is, the thickness change of the glass-ceramic before and after chemical strengthening is very small and can be ignored.
[0096] Density determination: The density of the microcrystalline glass sample was tested according to the principle of Archimedes' displacement method. The testing instrument used in this invention was an ALFA MIRAGE electronic density balance SD-200. To at least partially address the problem in related technologies where the optical and mechanical properties of microcrystalline glass cannot be effectively guaranteed due to the loss of crystallinity in exchange for a purer target crystalline phase, one embodiment of this application provides a precursor glass suitable for low-temperature crystallization treatment. The precursor glass can be understood as a raw glass or glass material obtained from melting glass raw materials. This precursor glass satisfies the following relationship: δ=a*n RO +b*(n Na2O +n K2O )+c*n Li2O , η=12.5 / (0.57+4.58*i^0.55929) 0.35≤δ / η≤0.69;
[0097] Where δ represents the ionic activity of each ion in the glass, η represents the correlation index between the kinetic energy of the thermal motion of oxide molecules in the glass and the characteristic temperature point, n represents the molar percentage content of each oxide, a, b, and c are constants, i is the characteristic temperature coefficient, 1.1 < a < 1.9, 1.5 < b < 2.7, 1.1 < c < 1.6, 5.29 < i < 9.73.
[0098] In an optional embodiment of this example, the value of δ / η can be 0.35, 0.37, 0.39, 0.41, 0.43, 0.45, 0.47, 0.49, 0.51, 0.53, 0.55, 0.57, 0.59, 0.61, 0.63, 0.65, 0.67, or 0.69. Furthermore, the range of δ / η can be 0.37–0.67, 0.39–0.65, 0.41–0.63, 0.43–0.61, 0.45–0.59, 0.47–0.57, 0.49–0.55, or 0.51–0.53. Preferably, the range of δ / η is 0.35–0.62.
[0099] It should be noted that i is the characteristic temperature coefficient, corresponding to the temperature of the characteristic viscosity point of the heat treatment process involved in the embodiments of this application. In practical applications, the characteristic temperature points of glass, such as the glass softening point, strain point, annealing point, and glass transition temperature, can be obtained through testing with a high-temperature rotational viscometer, plate viscometer, strain point and annealing point tester, linear dilatometer, differential scanning calorimeter (DSC), etc. These temperature points can then be tested, calculated, and fitted to obtain accurate temperatures. Finally, the viscosity-temperature curve can be obtained by fitting the viscosity and temperature using the VFT equation, thus yielding the temperature of the characteristic viscosity point.
[0100] The applicant's research revealed that alkali metals and alkaline earth metals significantly increase the crystallization tendency of glass, with Na₂O and K₂O exhibiting particularly prominent effects. This is because their small ionic radii make them more easily attracted to high-field ions under suitable temperature conditions. By introducing the δ calculation formula, oxides with different effects in glass can be classified and calculated. A comprehensive evaluation of different factors influencing crystallization tendency can describe the relationship between the electric field strength and ion migration of different oxides in glass. Furthermore, by introducing the η calculation formula, the relationship between the kinetic energy of the thermal motion of glass oxide molecules and characteristic temperature points is correlated with the aforementioned crystallization intensity, allowing for a comprehensive assessment of the crystallization tendency at lower temperatures.
[0101] In this embodiment, the glass crystallization tendency is characterized by describing the ionic activity of the glass using δ / η. By setting the value of δ / η within a specific range, it can be ensured that the glass viscosity is suitable for low-temperature crystallization. It is worth mentioning that the "suitable for low-temperature crystallization" mentioned in this embodiment means that the crystallization temperature required in this application embodiment is lower than the thermoforming and hot processing temperature, but high crystallinity can still be guaranteed. Since the crystallization temperature is relatively low, the generation of impurity phases can be effectively controlled.
[0102] In an optional embodiment of this example, the precursor glass also satisfies the following relationship: ε=A*n SiO2 +B*n B2O3 +C*n Al2O3 +D*n P2O5 +E*nRO + F*n R2O , 21.3≤ε≤25.6;
[0103] Where ε represents the degree of atomic packing, n represents the molar percentage content of each oxide, and A, B, C, D, E, and F are constants, with A = 26.1–28.3, B = 18.3–27.3, C = 40.2–42.7, D = 56.1–63.7, E = 12.2–22.6, and F = 10.9–36.2.
[0104] In an optional implementation of this embodiment, the value of ε can be 21.3, 21.5, 21.7, 21.9, 22.1, 22.3, 22.5, 22.7, 22.9, 23.1, 23.3, 23.5, 23.7, 23.9, 24.1, 24.3, 24.5, 24.7, 24.9, 25.1, 25.3, 25.5, 25.6. In optional embodiments, the value range of ε can also be: 21.5~25.5, 21.7~25.3, 21.9~25.1, 22.1~24.9, 22.3~24.7, 22.5~24.5, 22.7~24.3, 22.9~24.1, 23.1~23.9, 23.3~23.7. Preferably, the value range of ε is 22~24.5.
[0105] In an optional embodiment of this example, the formula for calculating the degree of atomic packing can be further expressed as: ε=A*n SiO2 +B*n B2O3 +C*n Al2O3 +D*n P2O5 +12.5* n MgO +14.4*n CaO +11.2*n Li2O +20.2*n Na2O +34*n K2O , 22.1≤ε≤24.5.
[0106] It should be noted that this embodiment uses an atomic packing degree calculation formula to control the glass component content, which can improve the chemical stability and impact resistance of the glass phase in the glass-ceramic.
[0107] It is worth mentioning that the formulas / relationships described above in this embodiment are essentially quantifications of the degree of change in glass viscosity and crystallization tendency related to composition. They can help understand the bond strength, coordination number, and connectivity of the glass structure network between anions and cations, thereby grasping the relationship between viscosity and glass composition. This can guide the glass crystallization temperature range and provide guidance for determining whether the glass formulation is suitable for low-temperature crystallization.
[0108] The precursor glass of this embodiment comprises, by molar percentage: 63% to 72% SiO2; 1.5% to 6% Al2O3; 16% to 26.8% Li2O; 0% to 6.5% Na2O; 0% to 4% K2O; 0.3% to 2.5% P2O5; 0% to 5% ZrO2; 0% to 5.3% RO, wherein RO includes at least one of CaO, MgO, ZnO, and BaO; and 0% to 1% clarifying agent.
[0109] SiO2 is the basic component of the glass composition provided in this application. It is the network structure form of glass and glass-ceramics, and can form lithium silicate and lithium disilicate after crystallization. It should be noted that if the SiO2 content is low, fewer crystals will form in the glass-ceramics, and the crystals will tend to be coarser, affecting the properties of the glass-ceramics and glass-ceramic products, such as haze and drop ball test height. Therefore, the lower limit of the SiO2 content is set at 63%. Conversely, if the SiO2 content is higher than a certain level, it will result in a high glass melting temperature, difficulty in material preparation, and difficulty in forming, affecting the consistency of the glass. Therefore, the upper limit of the SiO2 content is set at 72%. In some embodiments, the glass composition may contain approximately 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, 71%, or 72% SiO2. In some embodiments, the glass composition may also contain SiO2 in amounts such as 64% and less than or equal to 71%, 65% and less than or equal to 70%, 66% and less than or equal to 69%, or 67% and less than or equal to 68%.
[0110] Al2O3 can be a component forming the glass network structure or a cation network exogenous substance providing charge balance. In this application, all Al2O3 is incorporated into the glass network structure, increasing the depth of the ion exchange layer and surface compressive stress in the glass-ceramic product, thereby improving the chemical stability and mechanical properties of the glass. On the one hand, if its content is below a certain level, the effect will be unsatisfactory; therefore, the lower limit of the mass percentage content of Al2O3 is 1.5%. On the other hand, if the Al2O3 content is above a certain level, the melt permeability and devitrification resistance of the glass will decrease, and the crystals will tend to enlarge during crystallization, reducing the strength of the glass-ceramic and the glass-ceramic product; therefore, the upper limit of the Al2O3 content is 6%. In some embodiments, the glass composition may contain about 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, or 6% Al2O3. In some embodiments, the glass composition may also contain Al2O3 in amounts such as 2% and 5.5%, 2.5% and 5%, 3% and 4.5%, or 3.5% and 4.5%.
[0111] Li₂O is an essential component of the crystalline phases after crystallization, contributing to the formation of lithium-containing crystalline phases such as lithium disilicate, lithium feldspar, and lithium silicate. It is also a necessary component for chemical strengthening treatment. However, if its content is below a certain level, the effect is unsatisfactory. Therefore, the lower limit of Li₂O content is 16%. In addition, if its content is above a certain level, it will negatively affect the chemical stability of the glass. Therefore, the upper limit of Li₂O content is preferably 26.8%. In some embodiments, the glass composition may contain about 16%, 16.5%, 17%, 17.5%, 18%, 18.5%, 19%, 19.5%, 20%, 20.5%, 21%, 21.5%, 22%, 22.5%, 23%, 23.5%, 24%, 24.5%, 25%, 25.5%, 26%, 26.5%, and 26.8% Li₂O. In some embodiments, the glass composition may further contain Li2O in amounts such as: ≥16.5% and ≤26.5%, ≥17% and ≤26%, ≥17.5% and ≤25.5%, ≥18% and ≤25%, ≥18.5% and ≤24.5%, ≥19% and ≤24%, ≥19.5% and ≤23.5%, ≥20% and ≤23%, ≥20.5% and ≤22.5%, and ≥21% and ≤22%.
[0112] P2O5 helps improve the low-temperature melting properties of glass, enables phase separation and crystal nucleation in glass, and improves the thermal expansion stability of glass during crystallization. The lower limit of P2O5 content can be 0.3%. However, if there is too much P2O5, it can easily reduce the devitrification resistance of glass and cause phase separation, and the mechanical properties of glass tend to deteriorate. Therefore, the upper limit of P2O5 content is 2.5%. In some embodiments, the glass composition may contain about 0.3%, 0.5%, 1%, 1.5%, 2%, and 2.5% P2O5. In some embodiments, the glass composition may also contain P2O5 in the following amounts: greater than or equal to 0.5% and less than or equal to 2%, greater than or equal to 1% and less than or equal to 1.5%.
[0113] ZrO2 acts as a nucleating agent and also helps improve the chemical stability of the glass. In this embodiment, the lower limit of the ZrO2 content can be 0. However, if the ZrO2 content is too high, the devitrification resistance of the glass can easily decrease, and the glass crystallization process becomes more difficult to control, requiring a higher crystallization temperature. Therefore, the upper limit of the ZrO2 content is 5%. In some embodiments, the glass composition may contain approximately 0, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, or 5% ZrO2. In some embodiments, the glass composition may also contain ZrO2 in the following amounts: greater than or equal to 0.5% and less than or equal to 4.5%, greater than or equal to 1% and less than or equal to 4%, greater than or equal to 1.5% and less than or equal to 3.5%, or greater than or equal to 2% and less than or equal to 3%.
[0114] Na₂O helps lower the glass transition temperature and crystallization temperature, and suppresses the precipitation of unwanted impurity phases; its content can be limited to 0%. However, if the introduced Na₂O content is too high, it will increase the coefficient of thermal expansion of the glass and reduce its thermal stability; therefore, its content is limited to 6.5%. In some embodiments, the glass composition may contain about 0, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, and 6.5% Na₂O. In some embodiments, the glass composition may also contain Na₂O in the following amounts: greater than or equal to 0.5% and less than or equal to 6%, greater than or equal to 1% and less than or equal to 5.5%, greater than or equal to 1.5% and less than or equal to 5%, greater than or equal to 2% and less than or equal to 4.5%, greater than or equal to 2.5% and less than or equal to 4%, and greater than or equal to 3% and less than or equal to 3.5%.
[0115] Optionally, this embodiment also introduces K2O in a molar percentage of 0-4%, such as 0, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, or 4%. In some embodiments, the glass composition may also contain K2O in the following amounts: greater than or equal to 0.5% and less than or equal to 4%, greater than or equal to 1% and less than or equal to 3.5%, greater than or equal to 1.5% and less than or equal to 3%, or greater than or equal to 2% and less than or equal to 2.5%. It is worth mentioning that when multiple alkali metal oxides are present in the glass composition, a mixed alkali effect can be exerted during the chemical strengthening process of glass-ceramics. During ion diffusion, the migration of alkali metal ions can be restricted, which helps to improve the chemical stability of the glass. In addition, the interaction of multiple alkali metal oxides can improve the low-temperature melting and formability of the glass, and has a certain effect on reducing the softening point temperature and molding temperature of the glass, that is, reducing the difficulty of chemical strengthening of glass-ceramics.
[0116] RO is an alkaline earth metal oxide, including at least one selected from CaO, MgO, ZnO, and BaO. The lower limit of the alkaline earth metal oxide content is 0, and the upper limit is 5.3%. In some embodiments, the glass composition may contain about 0, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, and 5.3% of alkaline earth metal oxide. In some embodiments, the glass composition may also contain alkaline earth metal oxide in the following amounts: greater than or equal to 0.5% and less than or equal to 5%, greater than or equal to 1% and less than or equal to 4.5%, greater than or equal to 1.5% and less than or equal to 4%, greater than or equal to 2% and less than or equal to 3.5%, and greater than or equal to 2.5% and less than or equal to 3%.
[0117] In an optional embodiment of this example, the glass composition comprises: 0% to 4% CaO, 4% to 0% to 4% MgO, 4% to 0% to 4% ZnO, and 4% to 0% to 4% BaO. CaO helps reduce the high-temperature viscosity of the glass and increases its density; MgO helps reduce the viscosity of the glass, suppresses the tendency for crystallization during glass forming, and improves low-temperature melting properties; ZnO can improve the melting performance of the glass, improve its chemical stability, and refine the grains during crystallization; BaO can improve the glass-forming properties.
[0118] The glass composition of this embodiment may further include a clarifying agent, which includes one or more components selected from SnO2, Sb2O3, and CeO2. The lower limit of the clarifying agent content is 0%, and the upper limit is 1%. In some embodiments, the glass composition may contain about 0%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, or 1% of the clarifying agent. In some embodiments, the glass composition may also contain clarifying agents in the following amounts: greater than or equal to 0.1% and less than or equal to 0.9%, greater than or equal to 0.2% and less than or equal to 0.8%, greater than or equal to 0.3% and less than or equal to 0.7%, and greater than or equal to 0.4% and less than or equal to 0.6%.
[0119] In an optional embodiment of this example, the precursor glass composition, by molar percentage, further includes: greater than or equal to 0 and less than or equal to 4.8% B2O3; and / or, greater than or equal to 0 and less than or equal to 4% TiO2; and / or, greater than or equal to 0 and less than or equal to 4% Y2O3; and / or, greater than or equal to 0 and less than or equal to 0.5% La2O3.
[0120] B2O3 can lower the melting temperature of glass and, after crystallization, remains in the glass phase, ensuring structural stability and improving the chemical stability of glass-ceramics. However, excessive B2O3 content increases volatilization during glass melting, making glass homogenization more difficult. Therefore, the upper limit for B2O3 content is set at 4.8%. In some embodiments, the glass composition may contain approximately 0, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, or 4.8% B2O3. In some embodiments, the glass composition may also contain B2O3 in the following amounts: greater than or equal to 0.5% and less than or equal to 4.8%, greater than or equal to 1% and less than or equal to 4.5%, greater than or equal to 1.5% and less than or equal to 4%, greater than or equal to 2% and less than or equal to 3.5%, and greater than or equal to 2.5% and less than or equal to 3%.
[0121] TiO2 helps lower the melting temperature of glass and improve its chemical stability. By introducing TiO2 at a mass percentage of less than 4%, the glass crystallization process can be made easier to control. This embodiment optionally includes about 0, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, and 4% TiO2. In some embodiments, the glass composition may also contain TiO2 in amounts such as: greater than or equal to 0.5% and less than or equal to 3.5%, greater than or equal to 1% and less than or equal to 3%, and greater than or equal to 1.5% and less than or equal to 2.5%.
[0122] La2O3 and Y2O3 possess high field strength and an accumulation effect, strongly attracting surrounding non-bridging oxygen (NBO, i.e., broken Si-O- bonds), making the glass structure more compact. Simultaneously, they can form stronger La-O and YO bonds, improving the glass's chemical stability. La2O3 and Y2O3 are commonly used oxides in optical glasses, reducing dispersion and improving optical properties. In this embodiment, the glass composition optionally includes approximately 0, 0.1%, 0.15%, 0.25%, 0.3%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, and 4% La2O3 and / or Y2O3. In some embodiments, the glass composition may also contain La2O3 and / or Y2O3 in the following amounts: greater than or equal to 0% and less than or equal to 4%, greater than or equal to 0.1% and less than or equal to 3%, and greater than or equal to 0.15% and less than or equal to 0.3%.
[0123] Nb₂O₅ and Ta₂O₅ possess high field strength, which also improves chemical stability, reduces glass dispersion, and enhances optical performance. Among them, Ta₂O₅ has lower dispersion, higher Abbe number, and extremely strong corrosion resistance, which can significantly improve chemical stability. Nb₂O₅ simultaneously acts as a flux and increases glass hardness and scratch resistance. In this embodiment, it may optionally contain about 0, 0.1%, 0.15%, 0.25%, 0.3%, 0.5%, or 1% of Nb₂O₅ and / or Ta₂O₅. In some embodiments, the glass composition may also contain Nb₂O₅ and / or Ta₂O₅ in the following content ranges: greater than or equal to 0% and less than or equal to 1%, greater than or equal to 0.15% and less than or equal to 0.5%, and greater than or equal to 0.2% and less than or equal to 0.3%.
[0124] In addition to its high field strength, which improves chemical stability, HfO2 also has strong absorption of ultraviolet wavelengths, which can enhance radiation protection capabilities and has a significant effect on protecting human eye health. This embodiment optionally contains about 0, 0.1%, 0.15%, 0.25%, 0.3%, 0.5%, and 1% HfO2. In some embodiments, the glass composition may also contain HfO2 in the following content ranges: greater than or equal to 0% and less than or equal to 1%, greater than or equal to 0.15% and less than or equal to 0.5%, and greater than or equal to 0.2% and less than or equal to 0.3%.
[0125] Bi2O3 possesses extremely high refractive index and low dispersion properties, and also has a low melting point that can lower the glass crystallization temperature. In this embodiment, it optionally contains about 0, 0.1%, 0.15%, 0.25%, 0.3%, 0.5%, and 1% Bi2O3. In some embodiments, the glass composition may also contain Bi2O3 in the following content ranges: greater than or equal to 0% and less than or equal to 1%, greater than or equal to 0.15% and less than or equal to 0.5%, and greater than or equal to 0.2% and less than or equal to 0.3%.
[0126] In an optional embodiment of this example, the composition of the precursor glass is expressed as a molar percentage and satisfies at least one of the following relationships: 5 ≤ n Li2O / (n Na2O +n K2O )≤15; 7≤n Li2O / (n CaO +n MgO +n ZnO 0.25≤n ≤ 18; Li2O / (n SiO2 +n Al2O3 )≤0.5.
[0127] Li₂O, Na₂O, and K₂O are all alkali metal oxides. By adding these oxides in combination, a mixed alkali effect can be formed, improving the cross-linking density and chemical stability of the glass network, significantly enhancing the stability of glass-ceramic products. The Li₂O / (Na₂O+K₂O) ratio needs to meet certain ranges; if the (Na₂O+K₂O) ratio is too low, the mixed alkali effect cannot be formed, while if the (Na₂O+K₂O) ratio is too high, it will affect the formation ratio and rate of lithium crystals within the glass. (CaO+MgO+ZnO) has a high electric field strength. The proportion of (CaO+MgO+ZnO) can enhance the mechanical properties of glass, such as its elastic modulus and Vickers hardness. If the proportion of (CaO+MgO+ZnO) is too low, it will not achieve the beneficial effect of enhancing mechanical properties. If it is too high, it will promote the malignant growth of crystals and make it difficult to form microcrystals. (SiO2+Al2O3) is the main network forming body in glass and plays a decisive role in the viscosity and network crosslinking density of glass. If the proportion of (SiO2+Al2O3) is too low, it will not be possible to form controllable crystallization under suitable viscosity and temperature conditions. If the proportion is too high, it will affect the crystallinity and crystal size of glass, and at the same time make the glass viscosity too high, which is not conducive to production.
[0128] Next, this application embodiment also provides a microcrystalline glass, which is obtained by heat treatment (i.e., nucleation and crystallization treatment) of the aforementioned precursor glass. The lower limit temperature for crystallization of this microcrystalline glass is 553-639°C, and the upper limit temperature for crystallization is 989-1123°C. This microcrystalline glass satisfies at least one of the following performance indicators: Vickers hardness greater than or equal to 727 kgf / mm². 2Fracture toughness greater than or equal to 1.01 MPa·m 1 / 2 The properties are: Young's modulus greater than or equal to 99 GPa, shear modulus greater than or equal to 40 GPa, |B| value less than or equal to 0.74% at a thickness of 0.55 mm, haze less than or equal to 0.14%, and transmittance of visible light with a wavelength of 550 nm greater than or equal to 91%.
[0129] This application provides an exemplary first type of microcrystalline glass, the composition of which, in molar percentage, includes: 60% to 78% SiO2; 2% to 6.7% Al2O3; 16% to 24% Li2O; 0% to 2.2% P2O5; 0% to 5% ZrO2; 0% to 5.3% RO, wherein RO includes at least one of CaO, MgO, ZnO, and BaO; 0% to 5% Na2O; 0% to 4% K2O; and 0% to 1% clarifying agent.
[0130] The preferred content of SiO2 is 66–71.28%, a more preferred content is 66.5–70.8%, and a further preferred content is 67.1–69.5%; the preferred content of Al2O3 is 3–5.5%, a more preferred content is 3.5–5.2%, and a further preferred content is 3.5–4.6%; the preferred content of P2O5 is 0.3–1.6%, a more preferred content is 0.6–1.2%, and a further preferred content is 0.8–1.1%; and the preferred content of ZrO2 is 0–3%. The preferred content of Na₂O is 7%, more preferably 0-2.6%, and even more preferably 0.6-2.6%; the preferred content of Na₂O is 0-3.5%, more preferably 0-2.0%, and even more preferably 0-1.5%; the preferred content of K₂O is 0-2%, more preferably 0-0.5%, and even more preferably 0-0.3%; the preferred content of Li₂O is 18-23.5%, more preferably 20.5-23.5%, and even more preferably 21.5-23.5%. The aforementioned alkaline earth metal oxides, in this glass-ceramic, comprise: 0% to 4% CaO, 0% to 4% MgO, 0% to 4% ZnO, and 0% to 4% BaO. The preferred content of CaO is 0-2.5%, more preferably 0-1.5%, and even more preferably 0.2-0.5%. The preferred content of MgO is 0-2.5%, more preferably 0-1%, and even more preferably 0-0.5%. The preferred clarifying agent is SnO2, with a preferred content of 0.05-0.5%, more preferably 0.05-0.2%, and even more preferably 0.05-0.15%. In addition, the microcrystalline glass may further include: 0% to 4.8% B2O3, and / or 0% to 4% TiO2, and / or 0% to 4% Y2O3, and / or 0% to 0.5% La2O3, wherein the preferred content of B2O3 is 0-3%, more preferably 0-1.6%, and even more preferably 0-0.4%; the preferred content of TiO2 is 0-2.6%, more preferably 0-1.2%, and even more preferably 0-0.6%; the preferred content of Y2O3 is 0-2%, more preferably 0-0.5%, and even more preferably 0-0.3%; and the preferred content of La2O3 is 0-2%, more preferably 0-0.5%, and even more preferably 0-0.3%.
[0131] The microcrystalline glass has lithium disilicate and petalite as its crystal phases. The average grain size of the lithium disilicate phase is less than or equal to 32.5–39.3 nm, and the average grain size of the petalite phase is less than or equal to 24.6–29.1 nm. The crystallinity is greater than or equal to 84.72%. Furthermore, the lithium disilicate crystal phase meets the following criteria: 98% of the lithium disilicate crystal phase has a grain size less than or equal to 55 nm, 95% of the lithium disilicate crystal phase has a grain size less than or equal to 50 nm, and 80% of the lithium disilicate crystal phase has a grain size less than or equal to 45 nm; the lepidolite crystal phase meets the following criteria: 98% of the lepidolite crystal phase has a grain size less than or equal to 45 nm, 95% of the lepidolite crystal phase has a grain size less than or equal to 40 nm, and 80% of the lepidolite crystal phase has a grain size less than or equal to 30 nm; and the crystallinity is greater than or equal to 85.8%.
[0132] This application provides an exemplary embodiment of a second type of microcrystalline glass, the composition of which, in molar percentage, includes: 60% to 78% SiO2; 1.5% to 5.5% Al2O3; 18% to 26.8% Li2O; 0.1% to 2.5% P2O5; 0% to 5% ZrO2; 0% to 3.4% RO, wherein RO includes at least one of CaO, MgO, ZnO, and BaO; 0% to 6.5% Na2O; 0% to 4% K2O; and 0% to 1% clarifying agent.
[0133] The preferred content of SiO2 is 61.7–75.4%, a more preferred content is 62.4–71.3%, and an even more preferred content is 64.7–68.3%; the preferred content of Al2O3 is 2–5.5%, a more preferred content is 2–4.2%, and an even more preferred content is 2.5–3.5%; the preferred content of P2O5 is 0.6–2.5%, a more preferred content is 0.6–1.5%, and an even more preferred content is 1.0–1.4%; and the preferred content of ZrO2 is 0–3.7%. The preferred content of Na₂O is 0-2.6%, the more preferred content is 0.6-2.6%; the preferred content of Na₂O is 0-4.8%, the more preferred content is 0-3.1%, the more preferred content is 1.0-3.1%; the preferred content of K₂O is 0-2%, the more preferred content is 0-1.2%, the more preferred content is 0-0.6%; the preferred content of Li₂O is 18-25.8%, the more preferred content is 22.2-25.8%, the more preferred content is 23.4-24.4%. The aforementioned alkaline earth metal oxides, in this glass-ceramic, comprise: 0% to 4% CaO, 0% to 4% MgO, 0% to 4% ZnO, and 0% to 4% BaO. The preferred content of CaO is 0-2.5%, more preferably 0-1.5%, and even more preferably 0-0.5%. The preferred content of MgO is 0-2.5%, more preferably 0-1.5%, and even more preferably 0-0.5%. The preferred clarifying agent is SnO2, with a preferred content of 0.05-0.5%, more preferably 0.05-0.2%, and even more preferably 0.05-0.15%. In addition, the microcrystalline glass may further include: 0% to 4.8% B2O3, and / or 0% to 4% TiO2, and / or 0% to 4% Y2O3, and / or 0% to 0.5% La2O3, wherein the preferred content of B2O3 is 0-3%, more preferably 0-1.6%, and even more preferably 0-0.4%; the preferred content of TiO2 is 0-2.6%, more preferably 0-1.2%, and even more preferably 0-0.6%; the preferred content of Y2O3 is 0-2%, more preferably 0-0.5%, and even more preferably 0-0.3%; and the preferred content of La2O3 is 0-2%, more preferably 0-0.5%, and even more preferably 0-0.3%.
[0134] The crystalline phase of this glass-ceramic is lithium disilicate, which meets the following specifications: average grain size less than or equal to 38–45.7 nm, and crystallinity greater than or equal to 56.38%. Further, the lithium disilicate crystalline phase meets the following specifications: 98% of the grains in the overall crystalline phase have a size less than or equal to 60 nm, 95% of the grains in the overall crystalline phase have a size less than or equal to 55 nm, and 80% of the grains in the overall crystalline phase have a size less than or equal to 50 nm; crystallinity greater than or equal to 61.22%.
[0135] Next, this application embodiment also provides a chemically strengthened microcrystalline glass, which is obtained by sequentially subjecting the precursor glass provided in the foregoing embodiment to heat treatment and ion exchange treatment.
[0136] It is worth mentioning that the chemically strengthened microcrystalline glass of this embodiment meets at least one of the following performance indicators: Vickers hardness greater than or equal to 655 kgf / mm2, fracture toughness greater than or equal to 1.2 MPa·m1 / 2, Young's modulus greater than or equal to 98.38 GPa, shear modulus greater than or equal to 39.35 GPa, |B| value less than or equal to 0.74% when the thickness is 0.55 mm, haze less than or equal to 0.13%, transmittance relative to visible light with a wavelength of 550 nm greater than or equal to 91%, nine-point drop test height based on 32g steel ball with a thickness of 0.55 mm of 980-1290 mm, maximum bending strength of 1052-1200 MPa, whole machine drop test height based on 80-grit sandpaper of 850-1020 mm, and whole machine drop test height based on 180-grit sandpaper of 1200-1600 mm.
[0137] Accordingly, one embodiment of this application also provides a glass preparation method, which specifically includes:
[0138] Step A: After mixing the raw materials evenly according to the glass formula, melt them according to the preset melting temperature and melting time, and then anneal them to obtain the precursor glass.
[0139] Step B: Heat-treat the precursor glass to obtain glass-ceramic.
[0140] The precursor glass satisfies the following relationship: δ=a*n RO +b*(n Na2O +n K2O )+c*n Li2O , η=12.5 / (0.57+4.58*i^0.55929) 0.35≤δ / η≤0.69;
[0141] Where δ represents the ionic activity of each ion in the glass, η represents the correlation index between the kinetic energy of the thermal motion of oxide molecules in the glass and the characteristic temperature point, n represents the molar percentage content of each oxide, a, b, and c are constants, i is the characteristic temperature coefficient, 1.1 < a < 1.9, 1.5 < b < 2.7, 1.1 < c < 1.6, 5.29 < i < 9.73.
[0142] In practical applications, glass raw materials are first prepared according to the glass composition and content provided in the aforementioned embodiments. After the glass raw materials are mixed evenly, they are melted at 1350-1550°C. After clarification, homogenization, shaping, and annealing, precursor glass is obtained. Then, the precursor glass is crystallized using a two-stage heat treatment method. The first heat treatment is nucleation treatment, and the second heat treatment is crystallization treatment. After cooling to room temperature, microcrystalline glass with the expected crystallinity, grain size, and crystal phase ratio can be obtained.
[0143] The heat treatment process corresponding to the first type of microcrystalline glass provided in the foregoing embodiments may include: placing the glass raw material in a crystallization furnace, heating it to 500-610°C at a heating rate greater than or equal to 6°C / min and holding it at that temperature for 200-300 min, then heating it to 655-800°C at a heating rate greater than or equal to 6°C / min and holding it at that temperature for 60-120 min, and finally cooling it at a cooling rate less than or equal to 2°C / min.
[0144] Corresponding to the second type of microcrystalline glass provided in the aforementioned embodiments, its heat treatment process may include: placing the glass raw material in a crystallization furnace, heating it to 560-590°C at a heating rate of 8-12°C / min and holding it at that temperature for 220-250 min, then heating it to 750-790°C at a heating rate of 8-12°C / min and holding it at that temperature for 70-90 min, and finally cooling it at a cooling rate of less than or equal to 2°C / min.
[0145] Therefore, by using different heat treatment processes to heat-treat glass raw materials of different compositions, it is possible to obtain the desired type of crystal phase, desired crystal ratio, and desired grain size distribution.
[0146] It is worth mentioning that the microcrystalline glass obtained in step B above can be further subjected to cold processing, that is, through shaping, multi-wire cutting, CNC, grinding, rough grinding, fine polishing, cleaning and other processes, to obtain microcrystalline glass with a thickness of 0.35 to 0.7 mm.
[0147] In addition, corresponding to the second type of microcrystalline glass provided in the foregoing embodiments, this embodiment can also perform hot bending treatment on the microcrystalline glass, wherein the pressure of the hot bending workstation is 0.7 to 1.1 MPa, and the running time of a single workstation is 70 to 110 seconds.
[0148] In an optional embodiment of this example, the hot bending process requires four preheating stations, three hot pressing stations, and two cooling stations. The operating temperature of the first preheating station is 430–470°C, the second preheating station is 530–570°C, the third preheating station is 630–670°C, and the fourth preheating station is 710–730°C. The operating temperature of the first hot pressing station is 740–760°C, the second hot pressing station is 740–760°C, and the third hot pressing station is 580–620°C. The operating temperature of the first cooling station is 430–470°C, and the operating temperature of the second cooling station is 280–320°C.
[0149] In an optional embodiment of this example, the glass preparation method further includes: step C, immersing the microcrystalline glass in a chemically strengthened salt bath for ion exchange treatment to obtain chemically strengthened microcrystalline glass.
[0150] In this embodiment, when chemically strengthening the microcrystalline glass, the chemical strengthening salt bath comprises, by mass percentage: greater than or equal to 9.99% and less than or equal to 39.99% KNO3, greater than or equal to 59.99% and less than or equal to 89.99% NaNO3, and greater than or equal to 0.03% and less than or equal to 0.1% LiNO3. The temperature of the chemical strengthening salt bath is 460–490°C, and the duration of the ion exchange treatment is 4–10 hours.
[0151] Chemical strengthening refers to ion exchange treatment of glass-ceramics in a salt bath, resulting in the formation of compressive stress layers and tensile stress layers. In this embodiment, the salt bath is a mixed salt bath. Compared to traditional multiple strengthening processes, this embodiment can simultaneously complete multiple ion exchange processes between the salt bath and the glass-ceramics in a single strengthening step, improving chemical strengthening efficiency and reducing salt bath consumption. After chemical strengthening, the resulting chemically strengthened glass-ceramics exhibits a deeper compressive stress layer and higher surface compressive stress.
[0152] It is worth mentioning that for chemically strengthened glass-ceramics, after being removed from the salt bath, surface residues can be washed off first, followed by re-grinding using a flat grinder. The relevant parameters for the re-grinding process are set as follows: white grinding skin, hardness 75, upper and lower grinding disc speeds both 10 rpm, grinding powder concentration 1.13 g / cm³, pressure 150-250 kg, and 100-300 re-grinding cycles. Finally, the chemically strengthened glass-ceramics can be cleaned using a neutral cleaning agent with a pH of 7-9 to obtain chemically strengthened glass-ceramics products.
[0153] Corresponding to the first type of microcrystalline glass provided in the foregoing embodiments, the chemically strengthened microcrystalline glass obtained after ion exchange treatment meets the following performance indicators: surface compressive stress value of 255-280 MPa, compressive stress value at a depth of 50 μm from the surface of 105-112 MPa, compressive stress value at a depth of 80 μm from the surface of 65-70 MPa, compressive stress layer depth of 121-135 μm, absolute value of maximum tensile stress of 100-110 MPa, and absolute value of average tensile stress of 59-63 MPa.
[0154] Corresponding to the second type of microcrystalline glass provided in the foregoing embodiments, the chemically strengthened microcrystalline glass obtained after ion exchange treatment meets the following performance indicators: surface compressive stress value of 240-276 MPa, compressive stress value at a depth of 50 μm from the surface of 102-125 MPa, compressive stress value at a depth of 80 μm from the surface of 65-75 MPa, compressive stress layer depth of 113-130 μm, absolute value of maximum tensile stress of 105-108 MPa, and absolute value of average tensile stress of 58-63 MPa.
[0155] Next, in order to explain the technical effects of the precursor glass, microcrystalline glass, and chemically strengthened microcrystalline glass suitable for low-temperature crystallization in this embodiment, this application conducted tests on glass products with different component contents to determine their characteristics. Table 1 shows the relevant test conditions and test data of glass products with different component contents in this application.
[0156] Table 1
[0157] Table 2
[0158] On the one hand, as can be seen from Tables 1 and 2, the nucleation temperature and crystallization temperature of the microcrystalline glass in the embodiments of this application are in a relatively low range, that is, the heat treatment process implemented on the precursor glass is relatively mild. By controlling the glass viscosity, this application can ensure that the microcrystalline glass can achieve sufficient crystallization at low temperatures. On the other hand, referring to the mechanical property data (i.e., Vickers hardness, fracture toughness, Young's modulus, shear modulus, Poisson's ratio) and optical property data (i.e., refractive index, |B| value, haze, transmittance) provided in the embodiments in Tables 1 and 2 above, it can be seen that even if a relatively mild heat treatment process is used in the preparation of microcrystalline glass in order to control impurities, the final microcrystalline glass can still have high crystallinity and maintain relatively excellent mechanical and optical properties. In other words, this application creatively optimizes the glass composition ratio by considering the activity level of ions within the glass, the correlation between the thermal motion kinetic energy of oxide molecules in the glass and the characteristic temperature, and the degree of atomic packing. This allows the glass viscosity to be controlled, exhibiting a strong tendency to crystallize at low temperatures. This effectively overcomes the current problem in the production of microcrystalline glass where it is impossible to simultaneously control impurities and achieve mechanical and optical properties.
[0159] Figure 1 shows the DSC test curve of the microcrystalline glass corresponding to Example 4. In the DSC test spectrum of the prepared microcrystalline glass, the temperature of the first endothermic peak is 511.4℃ and the temperature of the first exothermic peak is 620℃. Figure 2 shows the XRD test curve of the microcrystalline glass corresponding to Example 4. It can be seen from the figure that the microcrystalline glass provided by this application has a lithium disilicate crystalline phase. Figure 3 shows the scanning electron microscope image of the microcrystalline glass corresponding to Example 4. It can be seen from the figure that the grain size of the lithium disilicate crystalline phase provided by this application is less than 60nm. Figure 4 shows the viscosity-temperature characteristics of the microcrystalline glass corresponding to Example 4, which is used to characterize the viscosity-temperature characteristics of the product.
[0160] It is also worth mentioning that, due to the superior performance of the chemically strengthened microcrystalline glass provided in the embodiments of this application, it can be widely used in the manufacture of protective covers for electronic devices, optical components, photovoltaic devices, or windows for household appliances.
[0161] Finally, it should be noted that the descriptions of each embodiment in the above embodiments have different focuses. For parts not described in detail in a certain embodiment, please refer to the relevant descriptions in other embodiments.
[0162] The above is a description of the precursor glass, glass-ceramic, chemically strengthened glass-ceramic, and glass preparation method provided in this application. For those skilled in the art, equivalent substitutions made in specific implementation methods and application scope based on the ideas of the embodiments of this application should be covered within the scope of the claims of this application. Therefore, the content of this specification should not be construed as a limitation on the solution of this application.
Claims
1. A precursor glass suitable for low temperature crystallization processing, characterized in that, The precursor glass satisfies the following relationship: δ = a*n RO +b*(n Na2O +n K2O )+c*n Li2O , η = 12.5 / (0.57+4.58*i0.55929) 0.35≤δ / η≤0.69; Where δ represents the ionic activity of each ion in the glass, η represents the correlation index between the kinetic energy of the thermal motion of oxide molecules in the glass and the characteristic temperature point, n represents the molar percentage content of each oxide, a, b, and c are constants, i is the characteristic temperature coefficient, 1.1 < a < 1.9, 1.5 < b < 2.7, 1.1 < c < 1.6, 5.29 < i < 9.
73.
2. The precursor glass of claim 1, wherein, The precursor glass also satisfies the following relationship: ε = A*n SiO2 + B*n B2O3 + C*n Al2O3 + D*n P2O5 + E*n RO + F*n R2O , 21.3 < ε < 25.6; Where ε represents the degree of atomic packing, n represents the molar percentage content of each oxide, and A, B, C, D, E, and F are constants, with A = 26.1–28.3, B = 18.3–27.3, C = 40.2–42.7, D = 56.1–63.7, E = 12.2–22.6, and F = 10.9–36.
2.
3. The precursor glass of claim 2, wherein, The precursor glass also satisfies the following relationship: ε = A*n SiO2 + B*n B2O3 + C*n Al2O3 + D*n P2O5 + 12.5*n MgO + 14.4*n CaO + 11.2*n Li2O + 20.2*n Na2O + 34*n K2O ; 22.1 < ε < 24.
5.
4. The precursor glass of claim 1, wherein, Its components, expressed as a mole percentage, include: SiO2 content greater than or equal to 63% and less than or equal to 72%; Al2O3 with a content greater than or equal to 1.5% and less than or equal to 6%; Li₂O content greater than or equal to 16% and less than or equal to 26.8%; Na₂O content greater than or equal to 0 and less than or equal to 6.5%; K₂O concentration greater than or equal to 0 and less than or equal to 4%; P2O5 content greater than or equal to 0.3% and less than or equal to 2.5%; ZrO2 greater than or equal to 0 and less than or equal to 5%; The content of RO is greater than or equal to 0 and less than or equal to 5.3%, and the RO includes at least one of CaO, MgO, ZnO and BaO; Clarifying agent with a concentration greater than or equal to 0 and less than or equal to 1%.
5. The precursor glass of claim 4, wherein, Its components, by mole percentage, also include: greater than or equal to 0 and less than or equal to 4.8% B2O3; and / or, greater than or equal to 0 and less than or equal to 2.6% TiO2; and / or, greater than or equal to 0 and less than or equal to 0.5% La2O3.
6. The precursor glass of claim 4, wherein, Its components, by mole percentage, include: greater than or equal to 1.5% and less than or equal to 5.5% Al2O3.
7. The precursor glass of claim 4, wherein, Its components, by molar percentage, include: greater than or equal to 0.6% and less than or equal to 1.6% P2O5.
8. The precursor glass of claim 4, wherein, Its components, in molar percentage, include: ≥16% and ≤26.8% Li2O, ≥0% and ≤4.5% Na2O, and ≥0% and ≤2% K2O.
9. The precursor glass of claim 8, wherein, Its components, by mole percentage, include: ≥22.2% and ≤25.8% Li2O, ≥0% and ≤3.1% Na2O, and ≥0% and ≤1.2% K2O.
10. The precursor glass of claim 9, wherein, Its components, by mole percentage, include: ≥20.5% and ≤23.5% Li2O, ≥0% and ≤2% Na2O, and ≥0% and ≤0.5% K2O.
11. The precursor glass further includes at least one of Y2O3, La2O3, Nb2O5, Ta2O5, HfO2, and Bi2O3.
12. The precursor glass of claim 4, wherein, The components of the precursor glass are in mole percent and satisfy at least one of the following relationships: 4≤n Li2O / (n Na2O +n K2O )≤17; 6≤n Li2O / (n CaO +n MgO +n ZnO )≤18; 0.24≤n Li2O / (n SiO2 +n Al2O3 )≤0.
38.
13. A glass-ceramic, characterized in that, The microcrystalline glass is obtained by heat treatment of the precursor glass according to any one of claims 1 to 11.
14. The glass-ceramic according to claim 13, characterized in that, The lower limit temperature for crystallization is 600–650℃, and the upper limit temperature for crystallization is 989–1123℃.
15. The glass-ceramic according to claim 13, characterized in that, The crystalline phase is lithium disilicate, and the lithium disilicate crystalline phase meets the following indicators: average grain size less than or equal to 38–45.7 nm, and crystallinity greater than or equal to 56.38%.
16. The glass-ceramic according to claim 15, characterized in that, The lithium disilicate crystal phase meets the following criteria: the size of 98% of the crystal phase is less than or equal to 60 nm, the size of 95% of the crystal phase is less than or equal to 55 nm, the size of 80% of the crystal phase is less than or equal to 50 nm, and the crystallinity is less than or equal to 68.22%.
17. The glass-ceramic according to any one of claims 13 to 16, characterized in that, satisfying at least one of the following performance indexes: Vickers hardness greater than or equal to 727 kgf / mm 2 , fracture toughness greater than or equal to 1.01 MPa·m 1 / 2 , Young's modulus greater than or equal to 99 GPa, shear modulus greater than or equal to 40 GPa, |B| value less than or equal to 0.75% when the thickness is 0.55 mm, haze less than or equal to 0.14%, transmittance greater than or equal to 91% with respect to visible light having a wavelength of 550 nm.
18. A chemically strengthened microcrystalline glass characterized in that, The chemically strengthened microcrystalline glass is obtained by sequentially subjecting the precursor glass according to any one of claims 1 to 11 to heat treatment and ion exchange treatment.
19. The chemically strengthened glass ceramic of claim 16, wherein, satisfying at least one of the following performance indexes: Vickers hardness greater than or equal to 655 kgf / mm 2 , fracture toughness greater than or equal to 1.2 Mpa.m 1 / 2 , Young's modulus greater than or equal to 98.38 GPa, shear modulus greater than or equal to 39.35 GPa, |B| value less than or equal to 0.8% when the thickness is 0.55 mm, haze less than or equal to 0.13%, transmittance greater than or equal to 91% relative to visible light with a wavelength of 550 nm, nine-point ball drop test height based on a 32 g steel ball of 980-1290 mm when the thickness is 0.55 mm, maximum bending strength of 1052-1200 MPa, whole machine drop test height based on 80 mesh sandpaper of 850-1020 mm, whole machine drop test height based on 180 mesh sandpaper of 1200-1600 mm.
20. A method of making glass, the method comprising: include: According to the glass formula, the raw materials are mixed evenly and then melted according to the preset melting temperature and melting time. After molding and annealing, the precursor glass is obtained. The precursor glass is heat-treated to obtain glass-ceramic. The precursor glass satisfies the following relationship: delta = a * n RO + b * (n Na2O + n K2O ) + c * n Li2O , η=12.5 / (0.57+4.58*i^0.55929) 0.35≤δ / η≤0.69; Where δ represents the ionic activity of each ion in the glass, η represents the correlation index between the kinetic energy of the thermal motion of oxide molecules in the glass and the characteristic temperature point, n represents the molar percentage content of each oxide, a, b, and c are constants, i is the characteristic temperature coefficient, 1.1 < a < 1.9, 1.5 < b < 2.7, 1.1 < c < 1.6, 5.29 < i < 9.
73.
21. The glass manufacturing method of claim 18, wherein, The heat treatment of the precursor glass includes: The precursor glass is placed in a crystallization furnace and heated to 500-610°C at a heating rate of 6°C / min or higher, and held for 200-300 min. Then, it is heated to 655-800°C at a heating rate of 6°C / min or higher, and held for 60-120 min. Finally, it is cooled at a cooling rate of 2°C / min or lower.
22. The glass manufacturing method of claim 18, wherein, The crystallization heat treatment of the precursor glass includes: The precursor glass is placed in a crystallization furnace and heated to 560-590°C at a heating rate of 8-12°C / min, and held at that temperature for 220-250 min. Then, it is heated to 750-790°C at a heating rate of 8-12°C / min and held at that temperature for 70-90 min. Finally, it is cooled at a cooling rate of less than or equal to 2°C / min.
23. The glass manufacturing method of claim 18, wherein, Also includes: The microcrystalline glass is subjected to hot bending treatment by a hot bending workstation; wherein the pressure of the hot bending workstation is 0.7 to 1.1 MPa, and the running time of a single workstation is 70 to 110 seconds.
24. The glass manufacturing method of claim 21, wherein, The hot bending process requires four preheating workstations, three hot pressing workstations, and two cooling workstations. The operating temperatures of the first preheating station are 430–470℃, the second preheating station is 530–570℃, the third preheating station is 630–670℃, the fourth preheating station is 710–730℃, the first hot pressing station is 740–760℃, the second hot pressing station is 740–760℃, the third hot pressing station is 580–620℃, the first cooling station is 430–470℃, and the second cooling station is 280–320℃.
25. The glass manufacturing method of claim 20, wherein, Also includes: The microcrystalline glass is immersed in a chemically strengthened salt bath for ion exchange treatment to obtain chemically strengthened microcrystalline glass. The chemically enhanced salt bath comprises, by mass percentage: 9.99% and 39.99% KNO3, 59.99% and 89.99% NaNO3, and 0.03% and 0.1% LiNO3.
26. The glass manufacturing method of claim 25, wherein, The temperature of the chemically enhanced salt bath is 460–490°C, and the duration of the ion exchange treatment is 4–10 hours.