Heavily-tungsten-doped cobalt hydroxide, and preparation method therefor and use thereof

The wet process for preparing highly tungsten-doped cobalt hydroxide solves the problems of uneven tungsten doping and low doping amount in existing technologies, achieving uniform doping of highly tungsten and low-cost preparation, which is suitable for preparing cathode materials.

WO2026237128A1PCT designated stage Publication Date: 2026-11-19GEM JIANGSU COBALT IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2025/102089
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-15
Filing Date
2025-06-19
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

In the preparation of cobalt hydroxide, existing technologies result in uneven tungsten doping and low doping levels. Furthermore, the use of ammonia water leads to complex wastewater treatment and long synthesis times, making it difficult to achieve uniform doping with high tungsten content.

Method used

A wet preparation method was adopted, using disodium ethylenediaminetetraacetate and/or citric acid as complexing agents. The cobalt salt and tungsten salt precipitant solution were mixed at high speed and vacuum dried to obtain highly tungsten-doped cobalt hydroxide. After calcination, uniformly doped cobalt tetroxide was obtained.

Benefits of technology

Uniform and high doping of tungsten was achieved, reducing preparation costs, simplifying wastewater treatment, and increasing the tungsten content to over 2.5 wt%. After calcination, the tungsten content in cobalt tetroxide was significantly increased, and the particles had small size and good dispersibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2025102089_19112026_PF_FP_ABST
    Figure CN2025102089_19112026_PF_FP_ABST
Patent Text Reader

Abstract

The present application relates to heavily-tungsten-doped cobalt hydroxide, and a preparation method therefor and the use thereof. The preparation method comprises the following steps: mixing a complexing agent solution of a cobalt salt with a precipitant solution of a tungsten salt under the condition of a rotational speed of 600 rpm or more, performing solid-liquid separation, and then performing washing and drying to obtain the heavily-tungsten-doped cobalt hydroxide. In the complexing agent solution of the cobalt salt, the complexing agent comprises ethylenediaminetetraacetic acid disodium salt and / or citric acid; and the amount of the precipitant solution of the tungsten salt is sufficient to make the content of tungsten in the heavily-tungsten-doped cobalt hydroxide reach 2.5 wt% or more. The preparation method provided in the present application can achieve the rapid preparation of heavily-tungsten-doped cobalt hydroxide. In addition, the preparation method used can achieve the uniform doping of tungsten.
Need to check novelty before this filing date? Find Prior Art

Description

A highly tungsten-doped cobalt hydroxide, its preparation method and application Technical Field

[0001] This application belongs to the field of battery materials technology, and relates to a cathode material, its preparation method and application, and particularly to a highly tungsten-doped cobalt hydroxide, its preparation method and application. Background Technology

[0002] Cobalt hydroxide is an inorganic compound, insoluble in water and sparingly soluble in strong alkalis, but soluble in acids and ammonium salt solutions. It has a wide range of applications in industrial production. For example, cobalt hydroxide can be used as a colorant for glass or enamel, providing a rose or light blue hue; it can be used as a drying agent in the coatings industry to improve the drying rate of paints; it can also be used in the chemical industry to manufacture cobalt salts or other cobalt compounds, and as a cobalt-containing catalyst; furthermore, it can be used as a decomposing agent in the electrolytic production of hydrogen peroxide; or as a cathode material in lithium batteries. Doping cobalt hydroxide with metal elements helps to improve its performance.

[0003] CN114671470A discloses a method for preparing tungsten-doped cobalt tetroxide and its application. The method involves dissolving a tungsten-containing compound and a molybdenum-containing compound in an alkaline solution to obtain a mixed solution. The mixed solution, a cobalt salt solution, and a complexing agent are then added concurrently to the base solution to initiate a reaction. The resulting precipitate is calcined under an oxygen atmosphere, and the calcined material is then immersed in a sodium sulfide solution to obtain tungsten-doped cobalt tetroxide. However, the synthesis process requires the use of 6 mol / L ammonia water as a complexing agent, and the resulting wastewater and toxic waste must be treated before discharge. Furthermore, the reaction time is relatively long, and tungsten doping can only be achieved with the participation of molybdenum.

[0004] CN110247029A discloses a method for preparing cobalt tetroxide with small particle size and high doping content of niobium, tungsten, and tantalum, including solution preparation, niobium-tungsten-tantalum crystal nucleus preparation, synthesis reaction, aging, filtration, washing, drying, and calcination. It achieves a high-concentration cobalt solution in the initial stage of synthesis. As the synthesis time increases, the concentration of the cobalt solution is reduced, increasing the number of cobalt hydroxide crystal nuclei generated in the initial stage of the synthesis reaction and inhibiting the growth rate of cobalt hydroxide. However, it requires the use of ammonia and hydrazine hydrate, and the tungsten doping amount can only reach 0.3%, making it difficult to achieve uniform tungsten doping.

[0005] Therefore, there is a need for a method and application of preparing highly tungsten-doped cobalt hydroxide that is simple to prepare, requires no ammonia, can achieve uniform tungsten doping, and has a high doping level. Summary of the Invention

[0006] The following is an overview of the subject matter described in detail herein. This overview is not intended to limit the scope of the claims.

[0007] In view of the shortcomings of the existing technology, the purpose of this application is to provide a highly tungsten-doped cobalt hydroxide, its preparation method and application. The preparation method can achieve rapid preparation of highly tungsten-doped cobalt hydroxide and can make the tungsten content above 2.5 wt%. In addition, the wet process used can make the tungsten doping uniform.

[0008] To achieve this objective, the present application adopts the following technical solution:

[0009] In a first aspect, this application provides a method for preparing highly tungsten-doped cobalt hydroxide, comprising the following steps:

[0010] At a rotational speed of 600 rpm or higher, the complexing agent solution of mixed cobalt salt and the precipitant solution of tungsten salt are separated into solid and liquid components, washed and dried to obtain the highly tungsten-doped cobalt hydroxide.

[0011] The complexing agent solution of the cobalt salt includes disodium ethylenediaminetetraacetate and / or citric acid;

[0012] The amount of the precipitant solution for the tungsten salt is such that the tungsten content in the highly tungsten-doped cobalt hydroxide reaches more than 2.5 wt%, and can reach up to 5.45 wt%.

[0013] In existing technologies for preparing cobalt tetroxide by tungsten doping, cobalt tetroxide and tungsten oxide are typically mechanically mixed using a dry method, resulting in uneven doping and low tungsten doping levels. Tungsten salts, precipitants, and cobalt salts compete for doping; high precipitant dosages make it difficult to achieve high tungsten doping, while low precipitant dosages, although increasing tungsten content, result in uneven distribution, low yield, and high cost. The preparation method provided in this application involves tungsten doping during the wet preparation of cobalt hydroxide, achieving uniform and high tungsten doping. Subsequent conventional calcination yields cobalt tetroxide with high and uniform tungsten doping.

[0014] In one embodiment, the concentration of cobalt in the complexing agent solution of the cobalt salt is 60 g / L to 120 g / L.

[0015] In one embodiment, the concentration of the complexing agent in the cobalt salt complexing agent solution is 0.8 g / L to 1.5 g / L.

[0016] In one embodiment, the cobalt salt complexing agent solution comprises cobalt sulfate and / or cobalt chloride.

[0017] In one embodiment, the precipitant solution of the tungsten salt includes any one or a combination of at least two of sodium metatungstate, sodium tungstate, sodium paratungstate, ammonium metatungstate, or ammonium tungstate.

[0018] In one embodiment, the precipitant solution of the tungsten salt includes sodium hydroxide.

[0019] In one embodiment, the volume ratio of the complexing agent solution of the cobalt salt to the precipitant solution of the tungsten salt is 15:1 to 32:1.

[0020] In one embodiment, the amount of the precipitant solution for the tungsten salt is such that the alkali-to-cobalt ratio is 2.1-4.

[0021] The alkali-cobalt ratio mentioned in this application refers to the molar ratio of the precipitant to the cobalt in the cobalt salt.

[0022] In one embodiment, the mixing includes: adding the precipitant solution of the tungsten salt to the complexing agent solution of the cobalt salt at a uniform rate within 3 minutes.

[0023] In one embodiment, the mixing is carried out in a protective atmosphere.

[0024] In one embodiment, the mixing temperature is below 25°C.

[0025] In one embodiment, the drying method includes vacuum drying.

[0026] In one embodiment, the vacuum drying temperature is 70°C-95°C.

[0027] Secondly, this application provides a highly tungsten-doped cobalt hydroxide, which is prepared by the preparation method described in the first aspect.

[0028] Thirdly, this application provides an application of the highly tungsten-doped cobalt hydroxide described in the second aspect, wherein the highly tungsten-doped cobalt hydroxide is used to prepare a cathode material.

[0029] The numerical range described in this application includes not only the point values ​​listed above, but also any point values ​​within the numerical ranges not listed above. Due to space limitations and for the sake of brevity, this application will not exhaustively list the specific point values ​​included in the range.

[0030] Compared with the prior art, this application has the following advantages:

[0031] In existing technologies for preparing cobalt tetroxide by tungsten doping, cobalt tetroxide and tungsten oxide are typically mechanically mixed using a dry method, resulting in uneven doping and low tungsten doping levels. This application reveals that tungsten salts, precipitants, and cobalt salts react in a competitive relationship. While high precipitant dosages can yield cobalt hydroxide, achieving high tungsten doping is difficult. Conversely, low precipitant dosages, while increasing tungsten content, result in uneven distribution, low yield, and high cost. The preparation method provided in this application incorporates tungsten doping during the wet preparation of cobalt hydroxide, achieving uniform and high tungsten doping. Subsequently, conventional calcination yields high-content, uniformly distributed tungsten-doped cobalt tetroxide.

[0032] After reading and understanding the accompanying diagrams and detailed descriptions, the other aspects can be understood. Attached Figure Description

[0033] The accompanying drawings are used to provide a further understanding of the technical solutions in this paper and form part of the specification. They are used together with the embodiments of this application to explain the technical solutions in this paper and do not constitute a limitation on the technical solutions in this paper.

[0034] Figure 1 is a SEM image of the highly tungsten-doped cobalt hydroxide obtained in Example 1 of this application;

[0035] Figure 2 is an EDS spot scan of the highly tungsten-doped cobalt hydroxide obtained in Example 1 of this application;

[0036] Figures 3 and 4 are EDS surface scans of the highly tungsten-doped cobalt hydroxide obtained in Example 1 of this application;

[0037] Figure 5 is a SEM image of the highly tungsten-doped cobalt hydroxide obtained in Example 2 of this application;

[0038] Figure 6 is an EDS spot scan of the highly tungsten-doped cobalt hydroxide obtained in Example 2 of this application;

[0039] Figures 7 and 8 are EDS surface scans of the highly tungsten-doped cobalt hydroxide obtained in Example 2 of this application;

[0040] Figure 9 is a SEM image of the highly tungsten-doped cobalt hydroxide obtained in Example 3 of this application;

[0041] Figure 10 is an EDS spot scan of the highly tungsten-doped cobalt hydroxide obtained in Example 3 of this application;

[0042] Figures 11 and 12 are EDS surface scans of highly tungsten-doped cobalt hydroxide obtained in Example 3 of this application;

[0043] Figure 13 is a SEM image of the highly tungsten-doped cobalt hydroxide obtained in Example 4 of this application;

[0044] Figure 14 is an EDS spot scan of tungsten-doped cobalt hydroxide obtained in Example 4 of this application;

[0045] Figure 15 is a SEM image of the tungsten-doped cobalt hydroxide obtained in Example 5 of this application;

[0046] Figures 16 and 17 are EDS surface scans of tungsten-doped cobalt hydroxide obtained in Example 5 of this application;

[0047] Figure 18 is a SEM image of the tungsten-doped cobalt hydroxide obtained in Example 6 of this application;

[0048] Figures 19 and 20 are EDS surface scans of the tungsten-doped cobalt hydroxide obtained in Example 6 of this application;

[0049] Figure 21 is a SEM image of the tungsten-doped cobalt hydroxide obtained in Example 7 of this application;

[0050] Figure 22 is an EDS spot scan of the tungsten-doped cobalt hydroxide obtained in Example 7 of this application;

[0051] Figure 23 is a SEM image of the tungsten-doped cobalt hydroxide obtained in Application Example 1 of this application;

[0052] Figure 24 is an EDS spot scan of the tungsten-doped cobalt hydroxide obtained in Application Example 1 of this application. Detailed Implementation

[0053] The technical solution of this application will be further described below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely to help understand this application and should not be regarded as specific limitations on this application.

[0054] This application provides a method for preparing highly tungsten-doped cobalt hydroxide, comprising the following steps:

[0055] At a rotational speed of 600 rpm or higher, the complexing agent solution of mixed cobalt salt and the precipitant solution of tungsten salt are separated into solid and liquid components, washed and dried to obtain the highly tungsten-doped cobalt hydroxide.

[0056] The complexing agent solution of the cobalt salt includes disodium ethylenediaminetetraacetate and / or citric acid;

[0057] The amount of the precipitant solution for the tungsten salt is such that the tungsten content in the highly tungsten-doped cobalt hydroxide reaches more than 2.5 wt%, and can reach up to 5.45 wt%.

[0058] In existing technologies for preparing cobalt tetroxide by tungsten doping, cobalt tetroxide and tungsten oxide are usually mechanically mixed by dry methods, resulting in uneven doping and low tungsten doping levels. The preparation method provided in this application, however, involves tungsten doping during the preparation of cobalt hydroxide, which enables uniform tungsten doping. Then, through conventional calcination, uniformly tungsten-doped cobalt tetroxide can be obtained, thereby achieving a high tungsten doping level in cobalt tetroxide.

[0059] In some embodiments, the concentration of cobalt in the complexing agent solution of the cobalt salt is 60 g / L-120 g / L, for example, it can be 60 g / L, 80 g / L, 90 g / L, 100 g / L or 120 g / L, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0060] In some embodiments, the concentration of the complexing agent in the cobalt salt complexing agent solution is 0.8 g / L to 1.5 g / L, for example, it can be 0.8 g / L, 0.9 g / L, 1 g / L, 1.2 g / L or 1.5 g / L, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0061] In some embodiments, the cobalt salt complexing agent solution comprises cobalt sulfate and / or cobalt chloride.

[0062] In some embodiments, the tungsten salt precipitant solution comprises any one or a combination of at least two of sodium metatungstate, sodium tungstate, sodium paratungstate, ammonium metatungstate, or ammonium tungstate. Typical but non-limiting combinations include combinations of sodium metatungstate and sodium tungstate, combinations of sodium metatungstate and sodium paratungstate, combinations of sodium metatungstate, sodium tungstate, and sodium paratungstate, combinations of ammonium metatungstate and ammonium tungstate, or combinations of sodium metatungstate, sodium tungstate, sodium paratungstate, ammonium metatungstate, and ammonium tungstate.

[0063] The complexing agent used in the preparation method provided in this application is not suitable for ammonia water, and there is no need to treat impurity ions such as ammonia nitrogen in wastewater.

[0064] In some embodiments, the precipitant solution of the tungsten salt includes sodium hydroxide.

[0065] In some embodiments, the volume ratio of the complexing agent solution of the cobalt salt to the precipitant solution of the tungsten salt is 15:1 to 32:1, for example, it can be 15:1, 18:1, 20:1, 24:1, 25:1, 28:1, 30:1 or 32:1, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0066] In some embodiments, the amount of the tungsten salt precipitant solution used is such that the alkali-cobalt ratio is 2.1-4, for example, it can be 2.1, 2.5, 2.8, 3, 3.2, 3.5 or 4, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0067] The alkali-cobalt ratio mentioned in this application refers to the molar ratio of the precipitant to the cobalt in the cobalt salt.

[0068] In some embodiments, the mixing includes: adding the precipitant solution of the tungsten salt to the complexing agent solution of the cobalt salt at a uniform rate within 3 minutes.

[0069] In some embodiments, the mixing is carried out in a protective atmosphere.

[0070] The protective atmosphere described in this application includes any one or a combination of at least two of nitrogen, helium, neon, or argon. Typical but non-limiting combinations include combinations of nitrogen and helium, helium and neon, neon and argon, helium, neon, and argon, or nitrogen, helium, neon, and argon.

[0071] In some embodiments, the mixing temperature is below 25°C, for example, it may be 20°C, 21°C, 22°C, 23°C, 24°C or 25°C, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0072] The preparation method provided in this application has a low mixing temperature and can achieve a high doping amount of tungsten with uniform doping.

[0073] In some embodiments, the drying method includes vacuum drying.

[0074] In some embodiments, the vacuum drying temperature is 70°C-95°C, for example, it can be 70°C, 75°C, 80°C, 85°C, 90°C or 95°C, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0075] One embodiment of this application provides highly tungsten-doped cobalt hydroxide, which is prepared by the preparation method described in any embodiment.

[0076] One embodiment of this application provides an application of the highly tungsten-doped cobalt hydroxide described in any embodiment, wherein the highly tungsten-doped cobalt hydroxide is used to prepare a cathode material.

[0077] For example, the preparation of cobalt tetroxide using the highly tungsten-doped cobalt hydroxide includes: calcining the highly tungsten-doped cobalt hydroxide to obtain the cobalt tetroxide.

[0078] In some embodiments, the calcination temperature includes 540°C-560°C, for example, 540°C, 545°C, 550°C, 555°C or 560°C, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0079] In some embodiments, the calcination time is 2h-4h, for example, it can be 2h, 2.5h, 3h, 3.5h or 4h, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0080] Example 1

[0081] This embodiment provides a method for preparing highly tungsten-doped cobalt hydroxide, the method comprising:

[0082] (1) Prepare a 10L cobalt salt complexing agent solution in a nitrogen atmosphere;

[0083] In the cobalt salt complexing agent solution, the cobalt salt is cobalt chloride, and the complexing agent is EDTA-2Na;

[0084] In the cobalt salt complexing agent solution, the concentration of cobalt is 60 g / L and the concentration of the complexing agent is 1 g / L;

[0085] (2) Add 1.98L of 32% sodium hydroxide solution (alkali-cobalt ratio of 2.1) and 90.29g of sodium tungstate dihydrate to 2L of water and mix well to obtain a tungsten salt precipitant solution.

[0086] (3) Under nitrogen atmosphere, adjust the rotation speed to 600 rpm and the temperature at 25°C, add the tungsten salt precipitant solution to the cobalt salt complexing agent solution at a uniform speed for 3 minutes.

[0087] (4) Solid-liquid separation, vacuum drying at 90°C to obtain high-tungsten-doped cobalt hydroxide with a tungsten content of 5.34wt%.

[0088] The SEM image of the highly tungsten-doped cobalt hydroxide obtained in this embodiment is shown in Figure 1, the EDS spot scan image is shown in Figure 2, and the ESD surface scan image is shown in Figures 3 and 4.

[0089] As shown in Figures 1-4, the highly tungsten-doped cobalt hydroxide obtained in this embodiment has a small particle size, a high tungsten content, and uniform doping.

[0090] Example 2

[0091] This embodiment provides a method for preparing highly tungsten-doped cobalt hydroxide, the method comprising:

[0092] (1) Prepare a 10L cobalt salt complexing agent solution in a nitrogen atmosphere;

[0093] In the cobalt salt complexing agent solution, the cobalt salt is cobalt chloride, and the complexing agent is EDTA-2Na;

[0094] In the cobalt salt complexing agent solution, the concentration of cobalt is 60 g / L and the concentration of the complexing agent is 0.8 g / L;

[0095] (2) Add 3.77L of 32% sodium hydroxide solution (alkali-cobalt ratio of 4) and 90.29g of sodium tungstate dihydrate to 2L of water and mix well to obtain a tungsten salt precipitant solution.

[0096] (3) Under nitrogen atmosphere, adjust the rotation speed to 600 rpm and the temperature at 25°C, add the tungsten salt precipitant solution to the cobalt salt complexing agent solution at a uniform speed for 3 minutes.

[0097] (4) Solid-liquid separation, vacuum drying at 80°C to obtain cobalt hydroxide with a tungsten content of 2.61 wt%.

[0098] The SEM image of the highly tungsten-doped cobalt hydroxide obtained in this embodiment is shown in Figure 5, the EDS spot scan image is shown in Figure 6, and the ESD surface scan image is shown in Figures 7 and 8.

[0099] As shown in Figures 5-8, the highly tungsten-doped cobalt hydroxide obtained in this embodiment has more flakes, lower tungsten content, and slightly uneven doping.

[0100] Example 3

[0101] This embodiment provides a method for preparing highly tungsten-doped cobalt hydroxide, the method comprising:

[0102] (1) Prepare a 10L cobalt salt complexing agent solution in a nitrogen atmosphere;

[0103] In the cobalt salt complexing agent solution, the cobalt salt is cobalt chloride, and the complexing agent is EDTA-2Na;

[0104] In the cobalt salt complexing agent solution, the concentration of cobalt is 120 g / L and the concentration of the complexing agent is 1.5 g / L;

[0105] (2) Add 3.96L of 32% sodium hydroxide solution (alkali-cobalt ratio of 2.1) and 180.59g of sodium tungstate dihydrate to 2L of water and mix well to obtain a tungsten salt precipitant solution.

[0106] (3) Under nitrogen atmosphere, adjust the rotation speed to 600 rpm and the temperature at 25°C, add the tungsten salt precipitant solution to the cobalt salt complexing agent solution at a uniform speed for 3 minutes.

[0107] (4) Solid-liquid separation, vacuum drying at 95°C to obtain high-tungsten-doped cobalt hydroxide with a tungsten content of 5.45wt%.

[0108] The SEM image of the highly tungsten-doped cobalt hydroxide obtained in this embodiment is shown in Figure 9, the EDS spot scan image is shown in Figure 10, and the ESD surface scan image is shown in Figures 11 and 12.

[0109] As shown in Figures 9-12, the highly tungsten-doped cobalt hydroxide obtained in this embodiment has a small particle size, good dispersibility, high tungsten content, and uniform doping.

[0110] Example 4

[0111] This embodiment provides a method for preparing highly tungsten-doped cobalt hydroxide, the method comprising:

[0112] (1) Prepare a 10L cobalt salt complexing agent solution in a nitrogen atmosphere;

[0113] In the cobalt salt complexing agent solution, the cobalt salt is cobalt sulfate, and the complexing agent is EDTA-2Na;

[0114] In the cobalt salt complexing agent solution, the concentration of cobalt is 60 g / L and the concentration of the complexing agent is 1.2 g / L;

[0115] (2) Add 1.98L of 32% sodium hydroxide solution (alkali-cobalt ratio of 2.1) and 69.80g of ammonium tungstate hexahydrate to 2L of water and mix well to obtain a tungsten salt precipitant solution.

[0116] (3) Under nitrogen atmosphere, adjust the rotation speed to 600 rpm and the temperature at 25°C, add the tungsten salt precipitant solution to the cobalt salt complexing agent solution at a uniform speed for 3 minutes.

[0117] (4) Solid-liquid separation, vacuum drying at 95°C to obtain highly tungsten-doped cobalt hydroxide with a tungsten content of 5.28 wt%.

[0118] The SEM image of the highly tungsten-doped cobalt hydroxide obtained in this embodiment is shown in Figure 13, and the EDS spot scan image is shown in Figure 14.

[0119] As shown in Figures 13 and 14, the highly tungsten-doped cobalt hydroxide obtained in this embodiment has a smaller particle size, a higher tungsten content, and uniform doping.

[0120] Example 5

[0121] This embodiment provides a method for preparing highly tungsten-doped cobalt hydroxide, the method comprising:

[0122] (1) Prepare a 10L cobalt salt complexing agent solution in a nitrogen atmosphere;

[0123] In the cobalt salt complexing agent solution, the cobalt salt is cobalt chloride, and the complexing agent is EDTA-2Na;

[0124] In the cobalt salt complexing agent solution, the concentration of cobalt is 60 g / L and the concentration of the complexing agent is 1.2 g / L;

[0125] (2) Add 5.66L of 32% sodium hydroxide solution (alkali-cobalt ratio of 6) and 90.29g of sodium tungstate dihydrate to 2L of water and mix well to obtain a tungsten salt precipitant solution.

[0126] (3) Under nitrogen atmosphere, adjust the rotation speed to 600 rpm and the temperature at 25°C, add the tungsten salt precipitant solution to the cobalt salt complexing agent solution at a uniform speed for 3 minutes.

[0127] (4) Solid-liquid separation, vacuum drying at 90°C to obtain highly tungsten-doped cobalt hydroxide with a tungsten content of 1.32 wt%.

[0128] The SEM image of the highly tungsten-doped cobalt hydroxide obtained in this embodiment is shown in Figure 15, and the ESD surface scan images are shown in Figures 16 and 17.

[0129] As shown in Figures 15-17, due to the excessively high alkali-cobalt ratio, the highly tungsten-doped cobalt hydroxide obtained in this embodiment has more flakes, larger particle size, poor dispersibility, and lower tungsten content.

[0130] Example 6

[0131] This embodiment provides a method for preparing highly tungsten-doped cobalt hydroxide, the method comprising:

[0132] (1) Prepare a 10L cobalt salt complexing agent solution in an air atmosphere;

[0133] In the cobalt salt complexing agent solution, the cobalt salt is cobalt chloride, and the complexing agent is EDTA-2Na;

[0134] In the cobalt salt complexing agent solution, the concentration of cobalt is 60 g / L and the concentration of the complexing agent is 1.2 g / L;

[0135] (2) Add 1.98L of 32% sodium hydroxide solution (alkali-cobalt ratio of 2.1) and 90.29g of sodium tungstate dihydrate to 2L of water and mix well to obtain a tungsten salt precipitant solution.

[0136] (3) Under air atmosphere conditions, adjust the rotation speed to 600 rpm and the temperature at 25°C, and add the tungsten salt precipitant solution to the cobalt salt complexing agent solution at a uniform speed for 3 minutes.

[0137] (4) Solid-liquid separation, vacuum drying at 90°C to obtain highly tungsten-doped cobalt hydroxide with a tungsten content of 2.74 wt%.

[0138] The SEM image of the highly tungsten-doped cobalt hydroxide obtained in this embodiment is shown in Figure 18, and the ESD surface scan images are shown in Figures 19 and 20.

[0139] As shown in Figures 18-20, the number of highly tungsten-doped cobalt hydroxide flakes obtained in this embodiment is less than that in Example 5, the particle size is still relatively large, the dispersibility is poor, and the tungsten doping content is increased.

[0140] Example 7

[0141] This embodiment provides a method for preparing highly tungsten-doped cobalt hydroxide, the method comprising:

[0142] (1) Prepare a 10L cobalt salt complexing agent solution in a nitrogen atmosphere;

[0143] In the cobalt salt complexing agent solution, the cobalt salt is cobalt chloride, and the complexing agent is EDTA-2Na;

[0144] The cobalt concentration in the complexing agent solution of the cobalt salt is 60 g / L;

[0145] (2) Add 1.98L of 32% sodium hydroxide solution (alkali-cobalt ratio of 2.1) and 90.29g of sodium tungstate dihydrate to 2L of water and mix well to obtain a tungsten salt precipitant solution.

[0146] (3) Under nitrogen atmosphere, adjust the rotation speed to 600 rpm and the temperature at 40°C, and add the tungsten salt precipitant solution to the cobalt salt complexing agent solution at a uniform speed for 3 minutes.

[0147] (4) Solid-liquid separation, vacuum drying at 90°C to obtain highly tungsten-doped cobalt hydroxide with a tungsten content of 2.24 wt%.

[0148] The SEM image of the highly tungsten-doped cobalt hydroxide obtained in this embodiment is shown in Figure 21, and the ESD spot scan image is shown in Figure 22.

[0149] As shown in Figures 21 and 22, due to the increased mixing temperature, the number of highly tungsten-doped cobalt hydroxide flakes obtained in this embodiment increased, while the tungsten content decreased.

[0150] Comparative Example 1

[0151] This comparative example provides a method for preparing highly tungsten-doped cobalt hydroxide, the method comprising:

[0152] (1) Prepare 10 L of cobalt salt solution in a nitrogen atmosphere;

[0153] In the cobalt salt solution, the cobalt salt is cobalt chloride;

[0154] The cobalt salt solution contains 60 g / L of cobalt.

[0155] (2) Add 1.98L of 32% sodium hydroxide solution (alkali-cobalt ratio of 2.1) and 90.29g of sodium tungstate dihydrate to 2L of water and mix well to obtain a tungsten salt precipitant solution.

[0156] (3) Under nitrogen atmosphere, adjust the rotation speed to 600 rpm and the temperature at 25°C, add the tungsten salt precipitant solution to the cobalt salt solution at a uniform speed for 3 minutes.

[0157] (4) Solid-liquid separation, vacuum drying at 90°C to obtain high-tungsten-doped cobalt hydroxide with a tungsten content of 1.75wt%.

[0158] Performance Characterization

[0159] The cobalt hydroxide obtained in the above examples and comparative examples was calcined at 550°C for 3 hours to obtain cobalt tetroxide. The tungsten content in the cobalt tetroxide obtained by calcining the highly tungsten-doped cobalt hydroxide obtained in Example 3 reached 6.20%. Its SEM image is shown in Figure 23 and its EDS spot scan image is shown in Figure 24. As can be seen from Figures 23 and 24, the tungsten content in the sample was significantly increased after calcination, the particle size was small, the dispersibility was good, and the tungsten was uniformly dispersed.

[0160] Cobalt tetroxide and lithium carbonate were mixed, and the molar ratio of Li to Co was controlled at 1.06:1. Then, solid-state sintering was carried out at 1000℃ for 12 hours to obtain lithium cobalt oxide cathode material.

[0161] Lithium cobalt oxide cathode material, acetylene black, and PVDF were mixed in a molar ratio of 92:4:4 and added to NMP to obtain a cathode slurry. This slurry was then coated onto aluminum foil to obtain a cathode sheet. A lithium sheet was used as the anode sheet, and CR2430 button batteries were fabricated in an argon-filled glove box. Electrical performance tests were performed using a Blue Electric testing system, including:

[0162] In laser particle size analysis, uniformity (also known as homogeneity) refers to the dispersion of particle size distribution in a sample, that is, the degree to which particle size deviates from the average value. This parameter reflects the concentration or dispersion of the particle population, similar to the concept of standard deviation in statistics. The smaller the value, the closer the particle size is to the average value, and the more uniform the particle size distribution.

[0163] The specific capacity was tested at room temperature, with a charge-discharge rate of 0.5C, a charge cut-off voltage of 4.3V, and a discharge cut-off voltage of 3.0V.

[0164] The test conditions for the first cycle capacity retention rate are the same as those for the specific capacity test, which is the first cycle discharge capacity / charge capacity.

[0165] Table 1

[0166] In summary, existing technologies for preparing cobalt tetroxide with tungsten doping typically involve dry mechanical mixing of cobalt tetroxide and tungsten oxide, resulting in uneven doping and low tungsten doping levels. Tungsten salts, precipitants, and cobalt salts compete for doping; while high precipitant dosages can yield cobalt hydroxide, achieving high tungsten doping is difficult. Conversely, low precipitant dosages, while increasing tungsten content, result in uneven distribution, low yield, and high cost. The preparation method provided in this application incorporates tungsten doping during cobalt hydroxide preparation, achieving uniform and high tungsten doping. Subsequent conventional calcination yields uniformly tungsten-doped cobalt tetroxide, thus achieving high tungsten doping in small-particle-size cobalt tetroxide.

[0167] The applicant declares that the above description is only a specific implementation of this application, but the protection scope of this application is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in this application fall within the protection and disclosure scope of this application.

Claims

1. A method for preparing highly tungsten-doped cobalt hydroxide, comprising the following steps: At a rotational speed of 600 rpm or higher, the complexing agent solution of mixed cobalt salt and the precipitant solution of tungsten salt are separated into solid and liquid components, washed and dried to obtain the highly tungsten-doped cobalt hydroxide. The complexing agent solution of the cobalt salt includes disodium ethylenediaminetetraacetate and / or citric acid; The amount of the precipitant solution for the tungsten salt is such that the tungsten content in the highly tungsten-doped cobalt hydroxide reaches more than 2.5 wt%.

2. The production method according to claim 1, wherein In the complexing agent solution of the cobalt salt, the concentration of cobalt is 60 g / L-120 g / L; Optionally, the concentration of the complexing agent in the cobalt salt complexing agent solution is 0.8 g / L to 1.5 g / L.

3. The production method according to claim 1 or 2, wherein The cobalt salt complexing agent solution contains cobalt sulfate and / or cobalt chloride.

4. The production process according to any one of claims 1 to 3, wherein The precipitant solution of the tungsten salt includes any one or a combination of at least two of sodium metatungstate, sodium tungstate, sodium paratungstate, ammonium metatungstate, or ammonium tungstate. Optionally, the precipitant in the tungsten salt precipitant solution includes sodium hydroxide.

5. The production process according to any one of claims 1 to 4, wherein The volume ratio of the complexing agent solution of the cobalt salt to the precipitant solution of the tungsten salt is 15:1-32:1; Optionally, the amount of the precipitant solution for the tungsten salt is such that the alkali-to-cobalt ratio is 2.1-4.

6. The method of making according to any one of claims 1-5, wherein, The mixing process includes adding the tungsten salt precipitant solution to the cobalt salt complexing agent solution at a uniform rate within 3 minutes.

7. The method of making according to any one of claims 1-6, wherein, The mixing is carried out in a protective atmosphere; Optionally, the mixing temperature is below 25°C.

8. The method of making according to any one of claims 1-7, wherein, The drying method includes vacuum drying; Optionally, the vacuum drying temperature is 70℃-95℃.

9. A highly tungsten-doped cobalt hydroxide prepared by the preparation method according to any one of claims 1-8.

10. An application of the highly tungsten-doped cobalt hydroxide of claim 9 in the preparation of cathode materials.