Battery device, electric device and energy storage device

By integrating without modules and optimizing the electrode structure, the heat dissipation capacity of the pouch cell is improved, solving the problem of heat accumulation in pouch cells during high-density integration, and achieving high capacity and improved safety performance of the battery device.

WO2026237156A1PCT designated stage Publication Date: 2026-11-19CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2025/107772
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-12
Filing Date
2025-07-09
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

When pouch cells are integrated at high density, their heat dissipation capacity is poor, leading to heat accumulation and potential safety hazards. This makes it difficult to simultaneously improve the capacity and safety performance of the battery device.

Method used

By adopting a module-free integration approach, the area ratio of small-diameter particles in the positive electrode film is adjusted to 8%-25%, combined with the conductive network of carbon nanotubes and conductive carbon black, the electrode structure and thermal management are optimized, and thermally conductive structural adhesives and thermal management components are used to improve heat dissipation efficiency.

Benefits of technology

It improves the overall capacity and safety performance of the battery device, reduces the probability of encapsulation failure, and enhances the cycle performance and reliability of individual pouch cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2025107772_19112026_PF_FP_ABST
    Figure CN2025107772_19112026_PF_FP_ABST
Patent Text Reader

Abstract

Provided in the present application are a battery device, an electric device and an energy storage device. The battery device comprises: a housing, which comprises a support plate and a frame; and a plurality of pouch battery cells, the rated capacity of the pouch battery cells being greater than or equal to 50 Ah and less than or equal to 300 Ah. At least one connecting beam is provided within the housing, and the pouch battery cells abut against the connecting beam. Each pouch battery cell comprises a packaging pouch, an electrode assembly and a current lead-out member, wherein the electrode assembly is accommodated within the packaging pouch; the electrode assembly comprises a positive electrode sheet; the positive electrode sheet comprises a positive current collector and a positive film layer arranged on at least one side of the positive current collector; the positive film layer comprises a positive active material; the positive active material comprises lithium-containing transition metal phosphate particles having at least part of their surfaces provided with a carbon material; in a cross-section of the positive film layer in the thickness direction of the electrode sheet, the area fraction of particles having a particle size greater than or equal to 50 nm and less than or equal to 250 nm is 8%-25%.
Need to check novelty before this filing date? Find Prior Art

Description

Battery devices, electrical devices and energy storage devices

[0001] Cross-referencing

[0002] This application claims priority to international patent application PCT / CN2025 / 094369, filed on May 12, 2025, entitled “Battery cell, battery device, power supply device and energy storage device”, the entire contents of which are incorporated herein by reference. Technical Field

[0003] This application relates to the field of battery technology, and in particular to a battery device, an electrical device, and an energy storage device. Background Technology

[0004] In recent years, the new energy industry has developed rapidly. As a core component of electric vehicles and energy storage systems, the performance of battery cells directly affects the range and safety of electrical devices. To meet market demand for high-capacity batteries, pouch cells have been widely used in the battery field due to their advantages such as light weight, flexible design, and high energy density. By optimizing the arrangement of multiple pouch cells, the integration of the battery system can be further improved, achieving a compact structure, thereby enhancing the overall energy density and range.

[0005] However, due to their soft-pack packaging, individual pouch cells have poor heat dissipation capabilities, easily accumulating heat during charging and discharging, leading to uneven temperature distribution. When multiple pouch cells are integrated at high density, the heat dissipation space is further limited, making it difficult to effectively dissipate heat. This can cause localized overheating, and even lead to safety hazards such as encapsulation failure and electrolyte leakage. In severe cases, it can even cause thermal runaway, deteriorating the safety and reliability of the battery device. Therefore, how to improve the safety performance of battery devices while increasing their capacity has become a key challenge that urgently needs to be overcome in the current battery technology field. Summary of the Invention

[0006] This application is made in view of the above-mentioned problems, and its purpose is to provide a battery device with high capacity and good safety performance.

[0007] This application provides a battery device, including a housing, a support plate, and a frame surrounding the outer periphery of the support plate, the support plate being fixedly connected to the frame; a plurality of pouch battery cells stacked in a first direction and housed within the housing; each pouch battery cell having a rated capacity greater than or equal to 50 Ah and less than or equal to 300 Ah; each pouch battery cell having a surface including a first surface and a second surface, the area of ​​the first surface being greater than the area of ​​the second surface, the first surfaces of the plurality of pouch battery cells being disposed opposite each other along the first direction, and the support plate and the second surfaces of the plurality of pouch battery cells being disposed opposite each other along a second direction; at least one connecting beam extending in a third direction is provided within the housing, the connecting beam being fixedly connected to the support plate and / or the frame, and at least one pouch battery cell abutting against the connecting beam along the first direction. The first direction, the second direction, and the third direction are perpendicular to each other; wherein, the soft-pack battery cell includes a packaging bag, an electrode assembly, and a current lead, the electrode assembly being housed within the packaging bag; one end of the current lead is connected to the electrode assembly, and the other end of the current lead is located outside the packaging bag, the current lead and the packaging bag being encapsulated and connected; the electrode assembly includes a positive electrode sheet, a negative electrode sheet, and a separator disposed between the positive electrode sheet and the negative electrode sheet, the positive electrode sheet including a positive current collector and a positive electrode film layer disposed on at least one side of the positive current collector, the positive electrode film layer including a positive active material, the positive active material including lithium transition metal phosphate particles with carbon material disposed on at least a portion of their surface; in the cross-section of the positive electrode film layer along the thickness direction of the electrode sheet, the area ratio of particles with a particle size greater than or equal to 50 nm and less than or equal to 250 nm is 8%-25%.

[0008] The enclosure, supported by a support plate and a frame around the support plate, helps reduce the weight of the battery pack, achieving lightweight design. However, this also weakens the stability of the battery pack. Including at least one connecting beam extending along a third direction within the enclosure, which abuts against the individual battery cells along the first direction, provides support to the cells. This improves the rigidity and structural stability of the battery pack while maintaining its lightweight design. Pouch batteries have low mechanical strength and poor resistance to internal pressure. Furthermore, with the integration of pouch battery cells into the enclosure in a module-less design, the lack of module separation between numerous cells means that the contamination caused by the failure of a single cell's encapsulation far exceeds that of traditional modules. Therefore, lithium transition metal phosphate systems, which offer high safety and relatively low gas production, are particularly suitable for pouch batteries.

[0009] However, lithium-containing transition metal phosphates are limited by specific capacity, requiring increased compaction to improve capacity and overcome the energy density bottleneck. Furthermore, when the rated capacity of a single pouch cell is less than 50 Ah, it is difficult to meet the power requirements of the battery device. When the rated capacity of a single pouch cell is greater than 300 Ah, higher capacity often requires thicker electrodes or larger electrode areas, and Joule heat and reaction heat increase significantly with increasing capacity, severely deteriorating the safety performance of the pouch cell. The applicant has discovered that a certain proportion of particle size distribution is beneficial to improving the compaction density of the positive electrode film, achieving a rated capacity of the pouch cell greater than or equal to 50 Ah and less than or equal to 300 Ah, ensuring a considerable overall capacity of the battery device. Specifically, when the area ratio of particles with a diameter greater than or equal to 50 nm and less than or equal to 250 nm in the cross-section along the thickness direction of the positive electrode film is less than 8%, insufficient particle size distribution will lead to limited improvement in compaction density, thus failing to meet the design requirements for the capacity of the pouch cell. The applicant also discovered that when the area ratio of particles with a diameter greater than or equal to 50 nm and less than or equal to 250 nm in the cross-section of the positive electrode film along the electrode thickness direction exceeds 25%, the excessively high proportion of small particles increases the interparticle interface, leading to an increase in electrode ohmic impedance. This, in turn, increases the internal resistance of the positive electrode film, exacerbates battery heat generation, hinders efficient heat diffusion from the tab to the interior of the electrode, and further increases the probability of encapsulation failure near the current lead. The embodiments of this application improve the battery device capacity by using lithium-containing transition metal phosphate pouch cell combined with a module-less integration method. Simultaneously, by controlling the area ratio of small-diameter lithium transition metal phosphate particles in the positive electrode film to within 8%-25%, the particle size distribution of the film is improved, while reducing the increase in resistance caused by excessive small particles. This reduces heat generation of the positive electrode during cycling, which is beneficial for improving the heat diffusion efficiency of heat conduction from the tab to the main electrode area. Heat is then dissipated through the first surface of the pouch battery and thermal management components, thereby reducing the probability of encapsulation failure near the current lead and improving the safety performance of the pouch battery cell. The embodiments of this application improve the overall capacity and safety performance of the battery device through a module-free integration method and the collaborative design of the pouch battery cell and the positive electrode.

[0010] In any embodiment, the rated capacity of the pouch battery cell is greater than or equal to 100Ah and less than or equal to 200Ah.

[0011] The rated capacity of the individual soft-pack battery cells is within the above-mentioned range, which is beneficial to improving the overall capacity of the battery device.

[0012] In any embodiment, in the cross-section of the positive electrode film layer along the electrode thickness direction, the area ratio of particles with a particle size greater than or equal to 50 nm and less than or equal to 250 nm is 8%-20%.

[0013] In the cross-section of the positive electrode film along the thickness direction of the electrode sheet, the area ratio of particles with a diameter greater than or equal to 50 nm and less than or equal to 250 nm is within the above range. This is beneficial to further reduce the resistance of the positive electrode film, reduce the heat generation of the positive electrode sheet during cycling, thereby improving the heat diffusion efficiency at the tab, and further reducing the probability of encapsulation failure near the current lead. The soft-pack battery cell has a high capacity while further improving the cycle performance of the soft-pack battery cell. The battery device with this soft-pack battery cell has good safety performance and high overall capacity.

[0014] In any embodiment, the median C of the graphitization degree C value in the cumulative distribution curve of the positive electrode film obtained in the laser microscopy confocal Raman spectroscopy instrument scanning mode is... 50 The value is 1.0-1.2, where the degree of graphitization C is I. G / I D , where I G This indicates that the Raman spectrum is at 1580±100 cm⁻¹ -1 The intensity of peak G at I D This indicates that the Raman spectrum is at 1350±100 cm⁻¹ -1 The intensity of peak D at that location.

[0015] In the cumulative distribution curve of graphitization degree C obtained by laser microscopy confocal Raman spectroscopy in instrument scanning mode, the median C of graphitization degree is... 50 Within the aforementioned range, the compaction density of the electrode sheet can be further increased by relying on particle slippage. This also helps to reduce the contact resistance between the positive electrode active material, the conductive agent, and the current collector, further reducing the heat generation of the positive electrode sheet during cycling. This improves the heat diffusion efficiency at the tab, thereby reducing the probability of encapsulation failure near the current lead. This is beneficial for improving the capacity of the pouch battery cell and further improving the cycle performance of the pouch battery cell, which in turn helps to improve the safety performance and overall capacity of the battery device.

[0016] In any embodiment, the positive electrode film layer further includes a conductive agent, the conductive agent including carbon nanotubes, the carbon nanotubes including one or more of single-walled carbon nanotubes, few-walled carbon nanotubes, and multi-walled carbon nanotubes, and the mass content of carbon nanotubes is 0.05%-2.5% based on the mass of the positive electrode film layer.

[0017] Carbon nanotubes can construct a three-dimensional network structure with shorter electron transport paths. Their fibrous structure can directly connect the current collector and the positive electrode active material, reducing the interfacial resistance between traditional conductive agents and positive electrode active materials. This helps to reduce the resistance of the positive electrode film. At the same time, the high coverage of its conductive network can reduce the probability of excessive local current density, thereby suppressing local temperature rise and further reducing the heat generation of the positive electrode during cycling. This improves the heat dissipation efficiency at the tabs, thereby reducing the probability of encapsulation failure near the current leads. This is beneficial to improving the cycle performance of pouch cell batteries and enhancing the safety performance of battery devices.

[0018] Within the aforementioned range, the carbon nanotube content helps reduce the probability of excessive agglomeration of the conductive agent due to excessive carbon nanotube content, ensuring its uniform distribution within the positive electrode film and the formation of a continuous and stable three-dimensional conductive network. This reduces the resistance of the positive electrode film, decreases heat generation during cycling, and improves heat dissipation efficiency at the tabs. Consequently, it reduces the probability of encapsulation failure near the current leads, further enhancing the cycle performance of the pouch cell and improving the safety performance of the battery device.

[0019] In any embodiment, the conductive agent further includes conductive carbon black, the mass content of which is 0.05%-2.5% based on the mass of the positive electrode film.

[0020] Conductive carbon black, with its small size, adheres to the surface of the positive electrode active material particles and fills the gaps between them, forming dense, dot-like conductive contacts. The combined use of carbon nanotubes and conductive carbon black balances both long-range and short-range conductivity, further improving the conductive network in the positive electrode film. This reduces the film's resistance, decreases heat generation during cycling, and enhances heat dissipation efficiency at the tabs, thereby reducing the probability of encapsulation failure near the current leads. This improves the cycle performance of individual pouch cells and enhances the safety of the battery system. Furthermore, conductive carbon black has a large specific surface area, which facilitates electrolyte absorption and retention, reducing electrolyte extrusion caused by high expansion forces during long cycles, further improving the cycle life of individual pouch cells.

[0021] When the mass content of conductive carbon black in the positive electrode film is within the above range, a more efficient conductive network is constructed by combining carbon nanotubes and conductive carbon black, optimizing the transport paths of electrons and ions, reducing polarization heat generation and Joule heat generation of the electrode, thereby improving the heat diffusion efficiency at the electrode tab, and further reducing the probability of encapsulation failure near the current lead-out component. This is beneficial to improving the cycle performance of the soft-pack battery cell and enhancing the safety performance of the battery device.

[0022] In any embodiment, based on the total area of ​​the cross-section of the positive electrode film layer along the thickness direction of the electrode sheet, the total area ratio of the agglomerated region of the conductive agent is 0.5%-2.5%, optionally 0.5%-2.0%; the agglomerated region of the conductive agent includes carbon nanotubes and conductive carbon black.

[0023] In this embodiment, the area ratio of the agglomerated region of the conductive agent is within the above-mentioned range. An appropriate amount of conductive agent agglomeration can form local high conductivity nodes, promote rapid electron transport, reduce ohmic impedance, thereby reducing the heat generation of the positive electrode, improving the heat diffusion efficiency at the tab, and further reducing the probability of encapsulation failure near the current lead, thereby further improving the cycle performance of the soft-pack battery cell and improving the safety performance of the battery device.

[0024] In any embodiment, the thickness of the positive electrode film layer on one side is 70μm-120μm.

[0025] The specific capacity of lithium-containing transition metal phosphate particles is relatively low. Studies have shown that when the single-sided thickness of the positive electrode film is less than 70 μm, the capacity of the battery cell is difficult to meet market demand. A single-sided thickness of the positive electrode film within the aforementioned range is beneficial for improving the capacity of pouch cell batteries. However, increasing the thickness of the positive electrode film leads to longer electron and ion transport paths, increased resistance of the positive electrode film, and increased ohmic and electrochemical heat generation on the positive electrode. Controlling the thickness of the positive electrode film within a reasonable range is beneficial for improving the capacity of pouch cell batteries and further improving their cycle performance.

[0026] In any embodiment, the thickness of the positive electrode film layer on one side is 90μm-120μm.

[0027] The thickness of the positive electrode film on one side within the above range is beneficial to further improve the capacity of the individual soft-pack battery cells, thereby increasing the overall capacity of the battery device.

[0028] In any embodiment, the thickness of the positive electrode film layer on one side is 100μm-120μm.

[0029] Increasing the thickness of the positive electrode film on one side is beneficial to improving the capacity of a single soft-pack battery cell. The applicant found that when the thickness of the positive electrode film on one side is greater than or equal to 100 μm, the positive electrode film is more prone to loosening and shedding of active material. The embodiments of this application contain an appropriate amount of small particles, so that the electrode sheet still has good compaction density while giving up a certain amount of large particles, reducing the probability of large particles rebounding and causing the positive electrode film to loosen and the active material to shed. The single soft-pack battery cell has high capacity and good cycle performance.

[0030] In any embodiment, when the pouch cell is fully discharged, the compaction density of the positive electrode sheet is 2.3 g / cm³.3 -2.6g / cm 3 .

[0031] When a single pouch cell is fully discharged, the compaction density of the positive electrode sheet is less than 2.3 g / cm³. 3 When the battery is in a state of insufficient interparticle connection, it not only fails to achieve ideal capacity performance, but also hinders the formation of electron conduction networks and lithium-ion transport channels, significantly increasing the battery's internal resistance and leading to increased ohmic heat generation. Furthermore, when the compaction density of the positive electrode sheet of a single battery cell in a fully discharged state exceeds 2.6 g / cm³, the battery will not achieve the desired capacity performance. 3 If the porosity of the positive electrode is too low, it will hinder lithium-ion diffusion and increase the electrochemical heat generation of the battery. Controlling the compaction density of the positive electrode within the above range is beneficial to improving the ohmic heat generation and electrochemical heat generation of the battery, thereby balancing the capacity and cycle performance of the pouch cell.

[0032] In any embodiment, the resistivity of the positive electrode film is 10 Ω·cm-35 Ω·cm.

[0033] This application embodiment controls the area ratio of small particles in the positive electrode film layer, so that the resistivity of the positive electrode film layer is in a low range. This helps to reduce electron transport impedance, reduce charge and discharge polarization, thereby reducing heat generation of the positive electrode during cycling. It also helps to conduct the heat accumulated at the tab to the main body area of ​​the electrode and achieve efficient heat dissipation through the electrode surface. This reduces the probability of encapsulation failure near the current lead, improves the safety and cycle performance of the soft-pack battery cell, and enhances the safety performance of the battery device.

[0034] In any embodiment, the diaphragm includes a base membrane, ceramic layers disposed on both sides of the base membrane, and an adhesive layer disposed on at least one side of the ceramic layer away from the base membrane. The adhesive layer is a continuous layer with a porous structure and includes a vinylidene fluoride polymer.

[0035] The separator provided in this application uses a continuous layer with a porous structure as the adhesive layer, which has a larger bonding area than the island-shaped adhesive layer in the prior art, thereby making the adhesion between the separator and the positive electrode film more firm and uniform. At the same time, thanks to the porous structure in the adhesive layer, it can also achieve lithium-ion transport efficiency and reduce electrochemical heat generation.

[0036] In this embodiment, a continuous layer with a porous structure is used as an adhesive layer to improve the adhesion between the separator and the electrode while maintaining the air permeability and porosity of the separator, thereby improving the compactness of the module, reducing the interface resistance, reducing the heat generation of the pouch cell during cycling, and improving the cycle performance of the pouch cell.

[0037] In any embodiment, the length dimension L0 of the soft-pack battery cell is 500mm-1250mm; the width dimension W0 is 100mm-150mm; and the thickness dimension H0 is 14mm-22mm.

[0038] The dimensions of the soft-pack battery cells in this application embodiment are within the above-mentioned range, which is beneficial for achieving better capacity of the battery cells and improving the overall capacity of the battery device.

[0039] In any embodiment, the packaging bag includes an encapsulation layer, a metal layer, and a protective layer stacked sequentially from the inside of the battery cell to the outside of the battery cell, wherein the metal layer comprises aluminum; and the encapsulation layer and the protective layer comprise resin material.

[0040] Packaging bag materials containing the above-mentioned components have high elongation, which helps to improve the space utilization of battery cells, thereby increasing the energy density and capacity of battery cells. However, the composite material composed of aluminum and resin has poor thermal conductivity, resulting in low heat dissipation efficiency of pouch battery cells. Therefore, if the area ratio of small particles in the positive electrode film is too high, it will increase the resistivity of the positive electrode film, leading to excessive heat generation during battery cycling and exacerbating the problem of poor heat dissipation in pouch battery cells. The embodiments of this application, by using the above-mentioned packaging bag and controlling the area ratio of small particles in the positive electrode film within a suitable range, achieve high capacity, good safety and cycle performance for pouch battery cells, and high overall capacity and good safety performance for the battery device.

[0041] In any embodiment, the encapsulation layer includes a polypropylene (PP) layer; optionally, the encapsulation layer includes a polypropylene (PP) layer and a modified polypropylene (PPa) layer disposed between the polypropylene (PP) layer and the metal layer; the protective layer includes one or more of nylon and polyethylene terephthalate (PET).

[0042] Modified polypropylene further improves the electrolyte corrosion resistance and bonding strength of the packaging bag. This encapsulation layer helps reduce interface leakage caused by insufficient heat sealing strength. The outer protective layer has excellent mechanical properties, which can buffer mechanical impact during assembly, reduce the risk of encapsulation failure of soft-pack battery cells, improve the safety performance of soft-pack battery cells, and thus improve the reliability of battery devices.

[0043] In any embodiment, the modified polypropylene (PPa) layer comprises maleic anhydride-grafted polypropylene.

[0044] Studies have shown that the main encapsulation failure sites near the current lead are the interfacial delamination between the polypropylene layer and the metal layer under high temperatures. The carboxyl groups (—COOH) and anhydride groups (—CO—O—CO—) of maleic anhydride can chemically bond with the hydroxyl groups (—OH) or alumina (Al2O3) on the aluminum foil surface, while simultaneously maintaining molecular chain entanglement with the polypropylene matrix. This helps to further improve the peel strength between the encapsulation layer and the metal layer, reducing the probability of delamination between the encapsulation layer and the metal layer under heat flow, lowering the risk of encapsulation failure in individual pouch cells, further improving the safety performance of pouch cell pouch cells, and enhancing the reliability of the battery device.

[0045] In any embodiment, the packaging bag is heat-sealed at 180°C-220°C.

[0046] The heat sealing temperature of the packaging bag is within the above range, which helps to enhance the interfacial bonding strength, reduce the probability of delamination between the encapsulation layer and the metal layer during battery cycling, reduce the risk of encapsulation failure of soft-pack battery cells, improve the safety performance of soft-pack battery cells, and improve the reliability of battery devices.

[0047] In any embodiment, the packaging bag is heat-sealed at 200°C-210°C.

[0048] The heat sealing temperature of the packaging bag is within the above range, which helps to further enhance the bonding strength between the encapsulation layer and the metal layer, thereby reducing the probability of delamination between the encapsulation layer and the metal layer during battery cycling, reducing the risk of encapsulation failure of soft-pack battery cells, improving the safety performance of soft-pack battery cells, and thus improving the reliability of battery devices.

[0049] In any embodiment, a thermally conductive structural adhesive is provided between the support plate of the housing and the soft-pack battery cell.

[0050] The thermally conductive structural adhesive of this application embodiment has good thermal conductivity and mechanical properties, which is beneficial for heat transfer from the soft-pack battery cell to the support plate for heat dissipation, thereby improving the cycle performance and safety performance of the soft-pack battery cell.

[0051] In any embodiment, a thermal management component is provided between the support plate of the housing and the second surface of the soft-pack battery cell. The thermal management component is used to regulate the temperature of the soft-pack battery cell, and a thermally conductive structural adhesive is provided between the thermal management component and the second surface of the soft-pack battery cell.

[0052] The heat from a single pouch battery cell can be efficiently dissipated through thermal management components, which helps to further improve the cycle performance and safety performance of the pouch battery cell.

[0053] In any embodiment, at 85°C, the thermal conductivity of the thermally conductive structural adhesive is greater than or equal to 0.4 W / (m·K), and can be selected as 0.4 W / (m·K)-1.2 W / (m·K).

[0054] In any embodiment, the thermal conductivity of the thermally conductive structural adhesive is 0.8 W / (m·K)-1.2 W / (m·K) at 85°C.

[0055] The thermal conductivity of the thermally conductive structural adhesive is within the above range, which has good thermal conductivity and can still conduct heat stably at high temperatures. This helps reduce the probability of thermally conductive structural adhesive failure due to temperature rise, which in turn leads to the inability of heat to be transferred from the pouch cell to the thermal management component or support plate for heat dissipation in time, resulting in heat accumulation inside the cell. This is beneficial to improving the cycle performance of the pouch cell during long-term cycling.

[0056] In any embodiment, the thermally conductive structural adhesive has a storage modulus of 260MPa-1000MPa at a vibration frequency of 0.1Hz at room temperature, and can be optionally 300MPa-800MPa.

[0057] In any embodiment, the thermally conductive structural adhesive has a storage modulus of 300MPa-600MPa at a vibration frequency of 0.1Hz at room temperature.

[0058] At room temperature, the energy storage modulus at a vibration frequency of 0.1 Hz is within the above range. It has good mechanical properties and can reduce the probability of creep deformation or fatigue cracking of the thermally conductive structural adhesive under long-term mechanical vibration. This reduces the probability of displacement of the soft-pack battery cell and loss of its own thermal conductivity caused by the deformation of the thermally conductive structural adhesive. The thermally conductive structural adhesive can give full play to its good thermal conductivity and further improve the cycle performance of the soft-pack battery cell in the long cycle process.

[0059] In any embodiment, the glass transition temperature of the thermally conductive structural adhesive is 50°C-60°C.

[0060] If the glass transition temperature of the thermally conductive structural adhesive is too low, when the operating temperature of the pouch cell exceeds this glass transition temperature, the energy storage modulus of the thermally conductive structural adhesive will drop sharply, causing the adhesive to transition from a glassy state to a viscoelastic state. After softening, the adhesive cannot provide sufficient mechanical holding force, and relative displacement or interfacial debonding may occur between the pouch cell and the thermal management components or support plate, reducing the thermal conductivity between the cell and the thermally conductive structural adhesive, and consequently reducing the heat dissipation efficiency of the cell. If the glass transition temperature of the thermally conductive structural adhesive is too high, at low temperatures, the adhesive remains in a glassy state, its toughness decreases, and the volume changes of the pouch cell during charging and discharging will generate stress at the interface, causing the thermally conductive structural adhesive to brittlely crack and develop fissures, resulting in a decrease in the heat dissipation efficiency of the cell.

[0061] When the glass transition temperature of the thermally conductive structural adhesive is within a suitable range, it is beneficial for the thermally conductive structural adhesive to fully exert its bonding and thermal conductivity, which is conducive to further improving the cycle performance of the soft-pack battery cells.

[0062] In any embodiment, the thermally conductive structural adhesive comprises a polyurethane resin and thermally conductive filler particles dispersed in the polyurethane resin; the thermally conductive filler particles comprise one or more of aluminum hydroxide particles and boron nitride particles.

[0063] Thermally conductive structural adhesives containing the above components exhibit good high-temperature resistance.

[0064] In any embodiment, based on the total mass of the thermally conductive structural adhesive, the mass percentage of the thermally conductive filler particles is 20%-70%, optionally 45%-65%.

[0065] The thermally conductive filler particles in the thermally conductive structural adhesive are within the above-mentioned range, which is beneficial to improving the thermal conductivity of the thermally conductive structural adhesive and reducing the problem of insufficient resin content caused by excessive thermally conductive filler particles, which would result in poor energy storage modulus of the thermally conductive structural adhesive. The thermally conductive structural adhesive has good thermal conductivity, which is beneficial to improving the cycle performance of soft-pack battery cells.

[0066] In any embodiment, the projection of the thermally conductive structural adhesive on the first surface does not overlap with the projection of the negative electrode sheet on the first surface.

[0067] After the battery cells are bonded to the thermally conductive structural adhesive, the adhesive may overflow. Once the battery cells are assembled into a battery device, the projection of the thermally conductive structural adhesive on the first surface does not overlap with the projection of the negative electrode sheet on the first surface. This reduces the probability of the relatively rigid thermally conductive structural adhesive and the electrode sheet directly compressing each other during battery cycling, lowering the probability of stress concentration on the battery electrode sheet caused by the thermally conductive structural adhesive, thereby reducing the adverse impact on the cycle performance of the pouch battery cells.

[0068] In any embodiment, at least some of the pouch cell units are provided with double-sided adhesive, and a gap is provided between the double-sided adhesive and the thermally conductive structural adhesive.

[0069] After the battery cells are bonded to the thermally conductive structural adhesive, excess adhesive may appear. The battery cells are then bonded together using double-sided adhesive. After assembling them into a battery device, a gap is created between the double-sided adhesive and the thermally conductive structural adhesive. This reduces the probability of the relatively rigid thermally conductive structural adhesive and the double-sided adhesive coming into contact with each other during battery cycling. This reduces stress concentration caused by the rigid thermally conductive structural adhesive on the double-sided adhesive between the battery cells, thereby minimizing any adverse impact on the cycle performance of the pouch battery cells.

[0070] A second aspect of this application provides an electrical device, including the battery device provided in the first aspect of this application, the battery device being used to provide electrical energy.

[0071] A third aspect of this application provides an energy storage device, including the battery device provided in the first aspect of this application, wherein the battery device is used to store electrical energy. Attached Figure Description

[0072] Figure 1 is a schematic diagram of a battery device according to an embodiment of this application;

[0073] Figure 2 is a partial enlarged view of a battery device according to an embodiment of this application;

[0074] Figure 3 is an enlarged view of the battery device shown in Figure 2 at box B;

[0075] Figure 4 is a partial enlarged view of a battery device according to another embodiment of this application;

[0076] Figure 5 is a schematic diagram of a battery cell according to an embodiment of this application;

[0077] Figure 6 is a cross-sectional view of the battery cell shown in Figure 5;

[0078] Figure 7 is an enlarged view of the battery cell shown in Figure 6 at box A;

[0079] Figure 8 is a schematic diagram of a packaging bag according to an embodiment of this application;

[0080] Figure 9 is a schematic diagram of an electrical device according to an embodiment of this application.

[0081] Explanation of reference numerals in the attached drawings: 10 Battery assembly; 1 Housing; 11 Support plate; 12 Connecting beam; 2 Soft-pack battery cell; 21 First surface; 22 Second surface; 201 Packaging bag; 202 Electrode assembly; 203 Current lead; 204 Tab; 221 Protective layer; 222 Metal layer; 223 Encapsulation layer; 3 Thermal management component; 4 Thermally conductive structural adhesive; X First direction; Y Second direction; Z Third direction. Detailed Implementation

[0082] The following detailed description, with appropriate reference to the accompanying drawings, specifically discloses embodiments of the battery device, power-consuming device, and energy storage device of this application. However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repetitive descriptions of practically identical structures may be omitted. This is to avoid unnecessarily lengthy descriptions and to facilitate understanding by those skilled in the art. Furthermore, the accompanying drawings and the following description are provided for the purpose of enabling those skilled in the art to fully understand this application and are not intended to limit the subject matter of the claims.

[0083] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values ​​of 1 and 2 are listed, and if maximum range values ​​of 3, 4, and 5 are listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0084] Unless otherwise specified, all embodiments and optional embodiments of this application may be combined with each other to form new technical solutions, and such technical solutions should be considered to be included in the disclosure of this application.

[0085] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions, and such technical solutions shall be deemed to be included in the disclosure of this application.

[0086] Unless otherwise specified, all steps in this application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the method may also include step (c), indicating that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.

[0087] In this application, the terms "multiple" or "various" refer to two or more kinds.

[0088] Unless otherwise stated, the terms used in this application have the common meanings as commonly understood by those skilled in the art.

[0089] Unless otherwise stated, the values ​​of the parameters mentioned in this application can be determined using various testing methods commonly used in the art, for example, according to the testing methods given in the embodiments of this application. Unless otherwise stated, the test temperature for each parameter is 25°C.

[0090] In embodiments of this application, the battery device includes multiple battery cell assemblies for providing voltage and capacity. A battery cell assembly may include multiple pouch cell batteries, which are connected in series, parallel, or mixed connections via a busbar. For example, a battery cell assembly is typically formed by arranging multiple pouch cell batteries; a battery cell assembly may also be a battery module, which is formed by arranging and fixing multiple pouch cell batteries into an independent module.

[0091] The battery device can be a battery pack, which includes a housing and multiple individual battery cells housed within the housing. The individual battery cells can be battery modules, which are housed within the housing by directly fixing multiple pouch cells to it.

[0092] In embodiments of this application, the housing can be part of the vehicle's chassis structure. For example, a portion of the housing can be at least a part of the vehicle's floor, or a portion of the housing can be at least a part of the vehicle's crossbeams and longitudinal beams.

[0093] In this embodiment, the battery cell can be a rechargeable battery, which refers to a battery cell that can be recharged after discharge to activate the active materials and continue to be used; the battery cell can be a lithium-ion battery. The battery cell can be flat.

[0094] In some implementations, the battery can be an energy storage device. Energy storage devices include energy storage containers, energy storage cabinets, etc.

[0095] In some embodiments, individual battery cells can be assembled into battery modules, and the number of battery cells contained in a battery module can be multiple, with the specific number adjustable according to the application and capacity of the battery module. In some embodiments, the above-mentioned battery modules can also be assembled into battery packs, and the number of battery modules contained in the battery packs can be adjusted according to the application and capacity of the battery packs.

[0096] A single battery cell includes electrode components and an electrolyte.

[0097] Electrode assemblies typically include positive and negative electrodes. The negative electrode is the electrode that absorbs or lithiates lithium ions during charging and releases or delithiates lithium during discharging. The positive electrode is the electrode that absorbs or delithiates lithium ions during charging and absorbs or lithiates lithium during discharging.

[0098] To meet the market demand for high-capacity battery devices, pouch cell batteries have advantages such as light weight, flexible design, and high energy density. Furthermore, the applicant discovered that by directly integrating multiple pouch cell batteries in a module-free manner, the traditional module structure is eliminated, and the reduction of redundant components helps to improve space utilization, thereby further increasing the battery capacity.

[0099] Soft-pack batteries are typically sealed in packaging bags with adhesive. Inside, they house electrode assemblies. These assemblies require current leads to connect to external circuits. The packaging bag is sealed to the current leads. The current leads conduct current, but the connection area between the current leads and the electrode assemblies is often limited, resulting in high current density and heat generation in the overcurrent region. The module-less design makes it even more difficult for heat to dissipate or be conducted quickly. Heat is rapidly transferred to the packaging bag at the connection point with the current leads. During high-rate charging and discharging or under long-term charging and discharging, the packaging bag and / or encapsulating adhesive near the current leads are prone to creep, leading to encapsulation failure in the vicinity of the current leads.

[0100] Such encapsulation failure can compromise the airtightness of individual battery cells, leading to battery performance degradation; it can even cause gases and liquid electrolytes generated by the thermal decomposition of the internal electrolyte to escape from the failure site, posing a safety risk. Simultaneously, the module-less integration method makes the arrangement of pouch cell batteries more compact, further limiting heat dissipation space and making heat more prone to accumulation, increasing the risk of heat seal failure and thermal runaway. How to obtain battery devices that simultaneously possess good capacity and safety performance is a pressing technical problem that needs to be solved in this field.

[0101] The first aspect of this application provides a battery device 10, as shown in Figures 1 to 7. The battery device 10 includes a housing 1; the housing 1 includes a support plate 11 and a frame surrounding the outer periphery of the support plate 11, the support plate 11 being fixedly connected to the frame; a plurality of pouch battery cells 2, the plurality of pouch battery cells 2 being stacked in a first direction X and housed within the housing 1; the rated capacity of the pouch battery cells 2 is greater than or equal to 50Ah and less than or equal to 300Ah; the surface of the pouch battery cells 2 includes a first surface 21 and a second surface 22, the area of ​​the first surface 21 being larger than the area of ​​the second surface 22, the first surfaces 21 of the plurality of pouch battery cells 2 being disposed opposite each other along the first direction X, the support plate 11 and the second surfaces 22 of the plurality of pouch battery cells 2 being disposed opposite each other along a second direction Y; at least one connecting beam 12 extending in a third direction Z is provided inside the housing 1, the connecting beam 12 being fixedly connected to the support plate 11 and / or the frame, at least one pouch battery cell 2 being disposed opposite to the support plate 11 along the first direction X. Connecting beam 12 abuts against each other, with the first direction X, the second direction Y, and the third direction Z being perpendicular to each other; wherein, the soft-pack battery cell 2 includes a packaging bag 201, an electrode assembly 202, and a current lead 203, the electrode assembly 202 being housed within the packaging bag 201; one end of the current lead 203 is connected to the electrode assembly 202, and the other end of the current lead 203 is located outside the packaging bag 201, with the current lead 203 and the packaging bag 201 being encapsulated and connected; the battery cell... The electrode assembly 202 includes a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode. The positive electrode includes a positive current collector and a positive electrode film layer disposed on at least one side of the positive current collector. The positive electrode film layer includes a positive active material, which includes lithium transition metal phosphate particles with carbon material disposed on at least a portion of their surface. In the cross-section of the positive electrode film layer along the thickness direction of the electrode, the area ratio of particles with a particle size greater than or equal to 50 nm and less than or equal to 250 nm is 8%-25%.

[0102] In this application, at least one of the soft-pack battery cells abutting against the connecting beam along the first direction means that the soft-pack battery cell and the connecting beam can be in direct or indirect contact, but the direction of the force between them is basically along the first direction.

[0103] The housing, supported by a support plate and a frame around the support plate, helps reduce the weight of the battery pack, achieving lightweight design. However, this also weakens the stability of the battery pack. At least one connecting beam extending along a third direction is provided inside the housing. This connecting beam abuts against the individual battery cells along a first direction, providing support to the battery cells. This improves the rigidity and structural stability of the battery pack while maintaining its lightweight design. It is understood that the statement that the support plate and the second surfaces of the multiple pouch battery cells are positioned opposite each other along a second direction means that the surfaces of the support plate and the second surfaces of the battery cells are opposite each other along the second direction, not necessarily that they are in contact. Similarly, the statement that the first surfaces of the multiple pouch battery cells are positioned opposite each other along the first direction does not necessarily mean that they are in direct or indirect contact.

[0104] In some embodiments, a thermal management component is provided between the support plate and the second surface of the plurality of pouch cell cells.

[0105] In some embodiments, the support plate is bonded to the second surface of the plurality of pouch cell cells.

[0106] Soft-pack batteries have low mechanical strength and poor resistance to internal pressure. Furthermore, after the soft-pack battery cells are integrated with the casing in a module-free design, there are no modules separating a large number of battery cells. The pollution caused by the failure of the encapsulation of a single battery cell is far greater than that of a traditional module. Therefore, lithium transition metal phosphate systems, which have high safety and relatively low gas production, are particularly suitable for soft-pack batteries.

[0107] However, lithium-containing transition metal phosphates are limited by specific capacity, requiring increased compaction to improve capacity and overcome the energy density bottleneck. Furthermore, when the rated capacity of a single pouch cell is less than 50 Ah, it is difficult to meet the power requirements of the battery device. When the rated capacity of a single pouch cell is greater than 300 Ah, higher capacity often requires thicker electrodes or larger electrode areas, and Joule heat and reaction heat increase significantly with increasing capacity, severely deteriorating the safety performance of the pouch cell. The applicant has discovered that a certain proportion of particle size distribution is beneficial to improving the compaction density of the positive electrode film, achieving a rated capacity of the pouch cell greater than or equal to 50 Ah and less than or equal to 300 Ah, ensuring a considerable overall capacity of the battery device. Specifically, when the area ratio of particles with a diameter greater than or equal to 50 nm and less than or equal to 250 nm in the cross-section along the thickness direction of the positive electrode film is less than 8%, insufficient particle size distribution will lead to limited improvement in compaction density, thus failing to meet the design requirements for the capacity of the pouch cell. The applicant also discovered that when the area ratio of particles with a diameter greater than or equal to 50 nm and less than or equal to 250 nm in the cross-section of the positive electrode film along the electrode thickness direction exceeds 25%, the excessively high proportion of small particles increases the interparticle interface, leading to an increase in electrode ohmic impedance. This, in turn, increases the internal resistance of the positive electrode film, exacerbates battery heat generation, hinders efficient heat diffusion from the tab to the interior of the electrode, and further increases the probability of encapsulation failure near the current lead. The embodiments of this application improve the battery device capacity by using lithium-containing transition metal phosphate pouch cell combined with a module-less integration method. Simultaneously, by controlling the area ratio of small-diameter lithium transition metal phosphate particles in the positive electrode film to within 8%-25%, the particle size distribution of the film is improved, while reducing the increase in resistance caused by excessive small particles. This reduces heat generation of the positive electrode during cycling, which is beneficial for improving the heat diffusion efficiency of heat conduction from the tab to the main electrode area. Heat is then dissipated through the first surface of the pouch battery and thermal management components, thereby reducing the probability of encapsulation failure near the current lead and improving the safety performance of the pouch battery cell. The embodiments of this application improve the overall capacity and safety performance of the battery device through a module-free integration method and the collaborative design of the pouch battery cell and the positive electrode.

[0108] In some implementations, end plates or side plates are provided on the frame.

[0109] In some implementations, neither end plates nor side plates are provided on the frame.

[0110] In some embodiments, as shown in FIG7, the electrode assembly 202 includes a tab 204, one end of a current lead 203 is connected to the tab 204, and the other end of the current lead 203 is located outside the packaging bag 201.

[0111] In this application, the rated capacity of a single pouch battery cell has a meaning known in the art, and can be tested using methods known in the art or obtained from the battery device instruction manual. As an example, at 25°C, the battery cell is charged to 3.65V at a charging rate of 0.5C (the nominal capacity of the cell), then charged at a constant voltage of 3.65V to 0.05C, left to stand for 10 minutes, and then discharged to 2.5V at a discharging rate of 1C, left to stand for 10 minutes. The capacity C during the discharge process is calculated using the formula C = I × t, with the unit being Ah.

[0112] Lithium-containing transition metal phosphate particles refer to phosphate materials containing lithium and transition metal elements, and can be detected by any method known in the art. For example, they can be detected by combining X-ray diffraction (XRD) with energy dispersive spectroscopy (EDS) or inductively coupled plasma mass spectrometry (ICP-MS).

[0113] It should be noted that the positive electrode film layer contains lithium transition metal phosphate particles, but the positive electrode film layer does not only refer to the positive electrode active material layer. Other film layers that are connected to the positive electrode active material layer and are difficult to distinguish, such as the undercoat layer and the liquid retention layer, are all collectively referred to as the positive electrode film layer.

[0114] In this application, the term "particle" refers to a particle in the positive electrode film layer that has a recognizable complete boundary in the field of view at a certain magnification, such as 10,000x. Defects and scratches may exist inside the particle, but a complete boundary sufficient to divide the particle cannot be identified inside the particle.

[0115] The particle identification method is as follows: The positive electrode film layer is cut along the thickness direction of the electrode sheet using an argon ion beam (for example, a Leica EM TIC 3X CP device can be used, operating voltage: 6kV, operating time: 6h). After exposing the cut surface, a scanning electron microscope (SEM) is used (for example, a Hitachi SU8230 device can be used, operating voltage: 3kV, beam current: high, probe model: U (LA100), working distance <5mm) to observe the cut surface along the thickness direction of the electrode sheet. Images are acquired using a field emission scanning electron microscope at a non-edge location in the cut surface of the positive electrode film layer (after observing the electrode edge under the SEM, the field of view is adjusted to the center of the sample) in secondary electron mode. Electron micrographs are taken at 10kx magnification, and the particles in the electron micrographs are analyzed using ImageJ software (1.46r, win64 version). The specific steps for using ImageJ software are as follows: Load the scanning electron microscope (SEM) image to be analyzed; use the Cellpose plugin to identify particles, and then perform manual corrections; use ImageJ to read and analyze data. The specific method for using the Cellpose plugin to identify particles is as follows: Set the segmentation diameter parameter (diameter in the Segmentation module) to 15 pixels, click "run cyto3" to identify particles; manually mark particles in the image that were not identified by the software, were not fully identified, or were identified incorrectly. Particles that were not identified by the software, were not fully identified, or were identified incorrectly mainly include the following: 1. Particles that are too large or have scratches on their surface, making them unidentifiable or incompletely identifiable; 2. During argon ion beam cutting, scratches may be generated on the particle surface, and the software may misinterpret these scratches as particle boundaries, leading to identification errors; 3. Particles that are too small and were not successfully identified; 4. Particles located at the edge of the SEM field of view, with the particle's interior penetrated by the edge, preventing a complete view of the morphology, resulting in identification errors due to partial identification replacing the whole.For the unidentified or misidentified particles mentioned above, manual calibration is performed. The specific process is as follows: 1. Delete large particles located around the edges of the scanning electron microscope that are not fully displayed. 2. Determine if any unidentified or misidentified particles have internal cracks or scratches. If no cracks or scratches are found, classify it as a single particle and manually mark it based on the observed particle boundary. 3. If cracks or scratches are found inside the particle, determine if they penetrate the particle. If not, classify it as a single particle and manually mark it. 4. If cracks or scratches penetrate the particle, determine if they are linear or irregular. 5. If the cracks or scratches are irregular, classify them as the boundary between particles and divide the particles along this boundary. 6. If the cracks or scratches are linear, perform contrast comparison. 7. If the contrast is not obvious and there is no crack-like appearance, classify it as a scratch and mark it as a single particle. 8. If the contrast is strong and there is a crack-like appearance, classify it as the boundary between particles and mark it as two particles. After manual marking, delete information irrelevant to the particles from the automatic image processing, thus completing the particle identification and marking in the image.

[0116] It is understandable that particles larger than 50 nm, especially in the cross-section of the positive electrode film along the electrode thickness direction, mainly originate from the positive electrode active material. Therefore, the embodiments of this application can accurately and objectively reflect the distribution of lithium transition metal phosphate particles within the positive electrode film by observing and statistically analyzing the particle area in the cross-section of the positive electrode film along the electrode thickness direction.

[0117] In existing technologies, laser particle size analyzers are typically used to statistically analyze the particle size of positive electrode active materials using Malvern laser diffraction. However, the applicant's research indicates that because lithium-containing transition metal phosphate particles are prone to agglomeration, the test results obtained by Malvern laser diffraction based on the principle of laser scattering often only reflect the particle size of the agglomerates, and cannot accurately reflect the particle size of the positive electrode active material, let alone its dispersion state in the film layer. This is because the dispersion of the positive electrode active material in the film layer increases during slurry preparation and film forming rolling. The test results obtained by Malvern laser diffraction are affected by the particle size, specific surface area, and degree of agglomeration of the positive electrode active material. Compared to the actual dispersion in the electrode sheet, the number of large particles obtained by this test is lower than the actual value, and the number of small particles is higher than the actual value. Therefore, the particle size obtained by Malvern laser diffraction cannot be equated with or analogized to the particle size statistically obtained in the embodiments of this application.

[0118] The specific method for testing the area ratio of particles with a diameter greater than or equal to 50 nm and less than or equal to 250 nm in the cross-section of the positive electrode film along the electrode thickness direction is as follows: Particles in the cross-section of the positive electrode film along the electrode thickness direction are identified according to the method described above in this application. The images after particle identification and labeling are imported into ImageJ software for analysis. The scale is set based on the scanning electron microscope image. The particle size, area, sphericity, and roughness of the particles in the cross-section along the electrode thickness direction are statistically analyzed using the "Feret," "Area," "Round," and "Solidity" analysis functions. According to the software manual (ImageJ User Guide IJ1.46r), the obtained "Feret" parameter represents the maximum spacing between all parallel lines in the two-dimensional projection of the particle, thus characterizing the particle size; the obtained "Area" parameter represents the pixel area of ​​the particle. Because particles smaller than 50 nm are prone to significant errors during statistical analysis and are difficult to accurately identify, and because the particle size of conductive agents is generally smaller than 50 nm, which can also introduce substantial errors into the statistical results, particles smaller than 50 nm are not counted in the particle size statistics process of this application. Furthermore, the statistical data for particles whose Area, Round, or Solidity is displayed as "NaN" are deleted. The sum of the "Area" parameters for particles with a diameter greater than or equal to 50 nm and less than or equal to 250 nm, and the sum of the "Area" parameters for all particles, are calculated and used as the area of ​​particles with a diameter greater than or equal to 50 nm and less than or equal to 250 nm, and the total area of ​​the counted particles, respectively. The sum of the areas of particles with a diameter greater than or equal to 50 nm and less than or equal to 250 nm, divided by the total area of ​​the counted particles, is used as the percentage of the area of ​​particles with a diameter greater than or equal to 50 nm and less than or equal to 250 nm in the cross-section of the positive electrode film along the thickness direction of the electrode sheet.

[0119] In some embodiments, the area percentage of particles with a diameter greater than or equal to 50 nm and less than or equal to 250 nm in the cross-section of the positive electrode film along the electrode thickness direction can be selected as 8%, 8.05%, 9%, 10%, 11%, 12%, 13%, 14%, 14.88%, 14.95%, 14.98%, 15%, 15.01%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 24.91%, 25%, or any value range between the two.

[0120] In some embodiments, the rated capacity of the pouch battery cell can be selected as 50Ah, 60Ah, 70Ah, 80Ah, 90Ah, 100Ah, 110Ah, 120Ah, 130Ah, 140Ah, 150Ah, 160Ah, 170Ah, 180Ah, 190Ah, 200Ah, 210Ah, 220Ah, 230Ah, 240Ah, 250Ah, 260Ah, 270Ah, 280Ah, 290Ah, 300Ah, or any value range between the two.

[0121] In some embodiments, the rated capacity of the pouch cell is greater than or equal to 100 Ah and less than or equal to 200 Ah.

[0122] The rated capacity of the individual soft-pack battery cells is within the above-mentioned range, which is beneficial to improving the overall capacity of the battery device.

[0123] In some embodiments, the area of ​​particles with a diameter greater than or equal to 50 nm and less than or equal to 250 nm in the cross-section of the positive electrode film along the thickness direction of the electrode sheet accounts for 8%-20%.

[0124] In the cross-section of the positive electrode film along the thickness direction of the electrode sheet, the area ratio of particles with a diameter greater than or equal to 50 nm and less than or equal to 250 nm is within the above range. This is beneficial to further reduce the resistance of the positive electrode film, reduce the heat generation of the positive electrode sheet during cycling, thereby improving the heat diffusion efficiency at the tab, and further reducing the probability of encapsulation failure near the current lead. The soft-pack battery cell has a high capacity while further improving the cycle performance of the soft-pack battery cell. The battery device with this soft-pack battery cell has good safety performance and high overall capacity.

[0125] In some embodiments, the median C of the graphitization degree C in the cumulative distribution curve of the positive electrode film obtained in laser microscopy confocal Raman spectroscopy instrument scanning mode is... 50 The value is 1.00-1.20; where the degree of graphitization C is I. G / I D I G This indicates that the Raman spectrum is at 1580±100 cm⁻¹ -1 The intensity of peak G at I D This indicates that the Raman spectrum is at 1350±100 cm⁻¹ -1 The intensity of peak D at that location.

[0126] In this application, the graphitization degree C value of the positive electrode film can be obtained by surface scanning mode of a laser confocal Raman spectrometer. As an example, specifically, a laser confocal Raman spectrometer (high-precision Renishaw laser confocal Raman spectrometer) is used, with an excitation wavelength of 532 nm. An appropriate amount of the positive electrode film is taken and surface scanned on its surface or along the thickness direction of the electrode. The scanning area is 45 μm × 45 μm, divided into 10 × 10 grids, with grid vertices as test points, a step size of 5 μm, and a total of 100 scan points. Thus, the C values ​​at different sites and the cumulative distribution curve of the C values ​​in the surface scan area are obtained.

[0127] The positive electrode film in this application can be either a freshly prepared positive electrode film or a positive electrode film obtained from disassembly of a battery. The surface of a positive electrode film obtained from disassembly of a battery inevitably contains residual electrolyte salt particles. To improve testing accuracy, it is preferable to perform a surface scan on a cross-section of the positive electrode film along the electrode thickness direction to characterize the degree of graphitization of the positive electrode film.

[0128] The graphitization degree C of the positive electrode film was obtained by the ratio of the peak intensities of the G-band and D-band in the Raman spectrum. The position of the G-band peak was 1580±100 cm⁻¹. -1 Its characterization of carbon sp 2 Hybrid structure; D peak position is 1350±100 cm⁻¹ - 1 It characterizes the disordered structure of carbon, where disorder refers to the irregular arrangement of carbon atoms in the structure.

[0129] The cumulative distribution curve of graphitization degree C value refers to the curve obtained by arranging at least 100 C values ​​in ascending order, with graphitization degree as the horizontal axis and the cumulative percentage as the vertical axis. 50 This represents the C value corresponding to a cumulative percentage of 50% on the vertical axis of the cumulative distribution curve of graphitization degree C. The median C value of graphitization degree. 50 Compared to point values, it can reflect the overall graphitization degree of particles in the positive electrode film, i.e., the degree of slippage; compared to the mean value, it can reduce the influence of extreme values ​​during the test and improve the confidence of the test results.

[0130] Those skilled in the art can control the degree of graphitization of active material particles using any known process. For example, adjusting the carbon source, sintering temperature, sintering time, sintering pressure, and sintering atmosphere can all achieve adjustments to the degree of graphitization of active material particles.

[0131] In some embodiments, the median C of the graphitization degree C in the cumulative distribution curve of the positive electrode film obtained in the laser microscopy confocal Raman spectroscopy instrument scanning mode is... 50The value can be selected from 1.0, 1.001, 1.002, 1.003, 1.006, 1.01, 1.02, 1.03, 1.04, 1.05, 1.06, 1.07, 1.08, 1.09, 1.1, 1.11, 1.12, 1.13, 1.14, 1.15, 1.16, 1.17, 1.18, 1.19, 1.20, or any value range between the two.

[0132] In the cumulative distribution curve of graphitization degree C obtained by laser microscopy confocal Raman spectroscopy in instrument scanning mode, the median C of graphitization degree is... 50 Within the aforementioned range, the compaction density of the electrode sheet can be further increased by relying on particle slippage. This also helps to reduce the contact resistance between the positive electrode active material, the conductive agent, and the current collector, further reducing the heat generation of the positive electrode sheet during cycling. This improves the heat diffusion efficiency at the tab, thereby reducing the probability of encapsulation failure near the current lead. This is beneficial for improving the capacity of the pouch battery cell and further improving the cycle performance of the pouch battery cell, which in turn helps to improve the safety performance and overall capacity of the battery device.

[0133] In some embodiments, the positive electrode film layer further includes a conductive agent, which includes carbon nanotubes, and the carbon nanotubes include one or more of single-walled carbon nanotubes, few-walled carbon nanotubes, and multi-walled carbon nanotubes. The mass content of carbon nanotubes is 0.05%-2.5% based on the mass of the positive electrode film layer.

[0134] In this application, the term "carbon nanotube" refers to a structure composed of carbon atoms arranged in sp... 2 Graphene sheets, formed by hybrid bonding, are rolled up to form nanomaterials with several to dozens of coaxial hollow cylindrical layers. Their diameters typically range from several to tens of nanometers, while their lengths can vary from micrometers to centimeters, exhibiting a high aspect ratio. Based on the number of layers, graphene sheets can be classified into: single-walled carbon nanotubes (SWCNTs), few-walled carbon nanotubes (FWCNTs), and multi-walled carbon nanotubes (MWCNTs). Carbon nanotubes possess excellent electrical conductivity and high elastic modulus.

[0135] Carbon nanotubes can construct a three-dimensional network structure with shorter electron transport paths. Their fibrous structure can directly connect the current collector and the positive electrode active material, reducing the interfacial resistance between traditional conductive agents and positive electrode active materials. This helps to reduce the resistance of the positive electrode film. At the same time, the high coverage of its conductive network can reduce the probability of excessive local current density, thereby suppressing local temperature rise and further reducing the heat generation of the positive electrode during cycling. This improves the heat dissipation efficiency at the tabs, thereby reducing the probability of encapsulation failure near the current leads. This is beneficial to improving the cycle performance of pouch cell batteries and enhancing the safety performance of battery devices.

[0136] In some embodiments, based on the mass of the positive electrode film, the mass content of carbon nanotubes can be selected as 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, or any value range between the two.

[0137] Within the aforementioned range, the carbon nanotube content helps reduce the probability of excessive agglomeration of the conductive agent due to excessive carbon nanotube content, ensuring its uniform distribution within the positive electrode film and the formation of a continuous and stable three-dimensional conductive network. This reduces the resistance of the positive electrode film, decreases heat generation during cycling, and improves heat dissipation efficiency at the tabs. Consequently, it reduces the probability of encapsulation failure near the current leads, further enhancing the cycle performance of the pouch cell and improving the safety performance of the battery device.

[0138] In some embodiments, the conductive agent further includes conductive carbon black, the mass content of which is 0.05%-2.5% based on the mass of the positive electrode film.

[0139] Conductive carbon black, with its small size, adheres to the surface of the positive electrode active material particles and fills the gaps between them, forming dense, dot-like conductive contacts. The combined use of carbon nanotubes and conductive carbon black balances both long-range and short-range conductivity, further improving the conductive network in the positive electrode film. This reduces the film's resistance, decreases heat generation during cycling, and enhances heat dissipation efficiency at the tabs, thereby reducing the probability of encapsulation failure near the current leads. This improves the cycle performance of individual pouch cells and enhances the safety of the battery system. Furthermore, conductive carbon black has a large specific surface area, which facilitates electrolyte absorption and retention, reducing electrolyte extrusion caused by high expansion forces during long cycles, further improving the cycle life of individual pouch cells.

[0140] In some embodiments, based on the mass of the positive electrode film, the mass content of conductive carbon black can be selected as 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, or any value range between the two.

[0141] When the mass content of conductive carbon black in the positive electrode film is within the above range, a more efficient conductive network is constructed by combining carbon nanotubes and conductive carbon black, optimizing the transport paths of electrons and ions, reducing polarization heat generation and Joule heat generation of the electrode, thereby improving the heat diffusion efficiency at the electrode tab, and further reducing the probability of encapsulation failure near the current lead-out component. This is beneficial to improving the cycle performance of the soft-pack battery cell and enhancing the safety performance of the battery device.

[0142] In some embodiments, the total area of ​​the agglomerated region of the conductive agent is 0.5%-2.5% based on the total area of ​​the cross-section of the positive electrode film along the thickness direction of the electrode sheet, and can be optionally 0.5%-2.0%; the agglomerated region of the conductive agent includes carbon nanotubes and conductive carbon black.

[0143] In this application, the area ratio of the conductive agent agglomeration region, based on the total area of ​​the cross-section of the positive electrode film layer along the electrode thickness direction, can be tested using the following method. A similar method to that described above is used to observe the cross-section of the positive electrode film layer along the electrode thickness direction using a scanning electron microscope (SEM), and the area of ​​the conductive agent agglomeration region in the SEM image is measured at 3kx magnification. Since the conductive agent is generally a carbon-based material, such as conductive carbon black or carbon nanotubes, aggregated conductive agent can be seen under high magnification in the SEM. The conductive agent agglomeration region often appears black and agglomerated compared to other areas in the positive electrode film layer. Using image analysis software, the conductive agent agglomeration region refers to the area in the SEM image where the conductive agent is clearly aggregated and appears black. Specifically, the scanning electron microscope (SEM) image at 3kx magnification is imported into ImageJ. Black conductive agent agglomeration regions with a Feret value greater than or equal to 2μm are selected, and the sum of the areas of these selected regions is recorded as the area of ​​the conductive agent agglomeration region. The area ratio of the conductive agent agglomeration region is the ratio of its area to the total area of ​​the imported SEM image. Three randomly selected, non-overlapping SEM images are used, and the average of these ratios is calculated as the "area ratio of the conductive agent agglomeration region based on the total area of ​​the cross-section along the electrode thickness direction of the positive electrode film."

[0144] In some embodiments, based on the total area of ​​the cross-section of the positive electrode film along the thickness direction of the electrode sheet, the area percentage of the agglomerated region of the conductive agent can be selected as 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, or any value range between the two.

[0145] Based on the total area of ​​the cross section along the thickness direction of the positive electrode film, the area ratio of the agglomerated region of the conductive agent is within the above range, indicating that the conductive agent in the positive electrode film is uniformly dispersed, which makes it easy to form a uniform conductive network. This reduces the probability of excessive current concentration caused by excessive agglomerated regions, which in turn leads to local overheating in the positive electrode, and is beneficial to improving the cycle performance of the pouch cell.

[0146] In some embodiments, the positive electrode film layer further includes a conductive agent, and the area of ​​the agglomerated region of the conductive agent accounts for 0.5%-2.0% based on the total area of ​​the cross section of the positive electrode film layer along the thickness direction of the electrode sheet.

[0147] In this embodiment, the area ratio of the agglomerated region of the conductive agent is within the above-mentioned range. An appropriate amount of conductive agent agglomeration can form local high conductivity nodes, promote rapid electron transport, reduce ohmic impedance, thereby reducing the heat generation of the positive electrode, improving the heat diffusion efficiency at the tab, and further reducing the probability of encapsulation failure near the current lead, thereby further improving the cycle performance of the soft-pack battery cell and improving the safety performance of the battery device.

[0148] In some embodiments, the agglomeration regions of the conductive agent include carbon nanotubes and conductive carbon black.

[0149] Researchers have discovered that carbon nanotubes, due to their high surface energy, are prone to aggregation, leading to uneven dispersion in the positive electrode film and hindering the formation of an effective carbon nanotube network structure. Conductive carbon black, with a surface energy similar to that of carbon nanotubes, can adsorb onto the carbon nanotube surface, forming a physical barrier that increases resistance to aggregation, reduces direct contact between carbon nanotubes, and thus inhibits aggregation. This improves the uniformity of carbon nanotube distribution in the positive electrode film, contributing to enhanced conductivity and improved electron and ion transport pathways. Furthermore, the aggregation of carbon nanotubes in conductive agent aggregation regions can cause localized blockage of ion transport pathways. The addition of conductive carbon black can improve lithium-ion transport capacity in these regions, reduce local polarization, decrease the probability of excessive localized heat generation, and further improve the cycle performance of individual pouch cell batteries.

[0150] In some implementations, the thickness of the positive electrode film on one side is 70 μm-120 μm.

[0151] The thickness of the positive electrode film can be measured using any method known in the art. As an example, the thickness of the positive electrode film in a cross-section along the thickness direction of the positive electrode sheet is measured using a scanning electron microscope. Measurements are taken at three randomly selected locations, and the average value is taken as the thickness of the positive electrode film.

[0152] In some embodiments, the thickness of one side of the positive electrode film can be selected as 70μm, 71μm, 72μm, 73μm, 74μm, 75μm, 76μm, 77μm, 78μm, 79μm, 80μm, 81μm, 82μm, 83μm, 84μm, 85μm, 86μm, 87μm, 88μm, 89μm, 90μm, 91μm, 92μm, 93μm, 94μm, 95μm, 96μm. m, 97μm, 98μm, 99μm, 100μm, 101μm, 102μm, 103μm, 104μm, 105μm, 106μm, 107μm, 108μm, 109μm, 110μm, 111μm, 112μm, 113μm, 114μm, 115μm, 116μm, 117μm, 118μm, 119μm, 120μm or any numerical range in between.

[0153] The specific capacity of lithium-containing transition metal phosphate particles is relatively low. Studies have shown that when the single-sided thickness of the positive electrode film is less than 70 μm, the capacity of the battery cell is difficult to meet market demand. A single-sided thickness of the positive electrode film within the aforementioned range is beneficial for improving the capacity of pouch cell batteries. However, increasing the thickness of the positive electrode film leads to longer electron and ion transport paths, increased resistance of the positive electrode film, and increased ohmic and electrochemical heat generation on the positive electrode. Controlling the thickness of the positive electrode film within a reasonable range is beneficial for improving the capacity of pouch cell batteries and further improving their cycle performance.

[0154] In some implementations, the thickness of the positive electrode film on one side is 90 μm-120 μm.

[0155] The thickness of the positive electrode film on one side within the above range is beneficial to further improve the capacity of the individual soft-pack battery cells, thereby increasing the overall capacity of the battery device.

[0156] In some implementations, the thickness of the positive electrode film on one side is 100 μm-120 μm.

[0157] Increasing the thickness of the positive electrode film on one side is beneficial to improving the capacity of a single soft-pack battery cell. The applicant found that when the thickness of the positive electrode film on one side is greater than or equal to 100 μm, the positive electrode film is more prone to loosening and shedding of active material. The embodiments of this application contain an appropriate amount of small particles, so that the electrode sheet still has good compaction density while giving up a certain amount of large particles, reducing the probability of large particles rebounding and causing the positive electrode film to loosen and the active material to shed. The single soft-pack battery cell has high capacity and good cycle performance.

[0158] In some embodiments, the compaction density of the positive electrode sheet of the pouch cell in its fully discharged state is 2.3 g / cm³. 3 -2.6g / cm 3 .

[0159] In this application, the fully discharged state refers to the state after the battery is placed in a 25°C oven environment, left to stand for 2 hours, and the battery temperature is maintained at 25°C, and then discharged at a constant current of 1 / 3C to 2.5V and then discharged at a constant current of 0.1C to 2.0V.

[0160] The compaction density of the positive electrode sheet can be tested using methods known in the art. As an example, the battery is placed in a 25°C oven environment and left to stand for 2 hours. After the battery temperature is maintained at 25°C, the battery is discharged at a constant current of 1 / 3C to 2.5V and then discharged at a constant current of 0.1C to 2.0V. The battery is then disassembled to obtain the positive electrode sheet. The residual electrolyte is treated with dimethyl carbonate solvent, the electrode sheet is dried, and it is cut into small circular pieces with an area of ​​S. The mass of the circular pieces is obtained as W1, and the thickness of the positive electrode sheet is measured using a micrometer. Then, the positive electrode film layer of the weighed electrode sheet is wiped off, the mass of the current collector is weighed and recorded as W2, and the thickness of the current collector is measured using a micrometer. Then, the compaction density of the positive electrode sheet is PD=(W1-W2) / [(T1-T2)×S].

[0161] In some embodiments, the compaction density of the positive electrode sheet of a single pouch cell in its fully discharged state can be selected as 2.3 g / cm³. 3 2.31 g / cm 3 2.32 g / cm 3 2.33 g / cm 3 2.34 g / cm 3 2.35g / cm 3 2.36 g / cm 3 2.37 g / cm 3 2.38g / cm 3 2.39 g / cm 3 2.40 g / cm 3 2.41 g / cm 3 2.42 g / cm 32.43 g / cm 3 2.44 g / cm 3 2.45g / cm 3 2.46 g / cm 3 2.47 g / cm 3 2.48 g / cm 3 2.49 g / cm 3 2.50g / cm 3 2.51g / cm 3 2.52g / cm 3 2.53g / cm 3 2.54 g / cm 3 2.55g / cm 3 2.56 g / cm 3 2.57g / cm 3 2.58g / cm 3 2.59g / cm 3 2.60g / cm 3 Or the range of values ​​between any two.

[0162] When a single pouch cell is fully discharged, the compaction density of the positive electrode sheet is less than 2.3 g / cm³. 3 When the battery is in a state of insufficient interparticle connection, it not only fails to achieve ideal capacity performance, but also hinders the formation of electron conduction networks and lithium-ion transport channels, significantly increasing the battery's internal resistance and leading to increased ohmic heat generation. Furthermore, when the compaction density of the positive electrode sheet of a single battery cell in a fully discharged state exceeds 2.6 g / cm³, the battery will not achieve the desired capacity performance. 3 If the porosity of the positive electrode is too low, it will hinder lithium-ion diffusion and increase the electrochemical heat generation of the battery. Controlling the compaction density of the positive electrode within the above range is beneficial to improving the ohmic heat generation and electrochemical heat generation of the battery, thereby balancing the capacity and cycle performance of the pouch cell.

[0163] In some implementations, the resistivity of the positive electrode film is 10 Ω·cm to 35 Ω·cm.

[0164] The resistivity of the positive electrode film can be tested by the following method: a resistance tester (Suzhou Lidian) is used to test under a standard pressure of 25MPa. During the test, 8 test points are randomly selected on the film of the positive electrode sheet. The pressure is maintained at each test point for 15s to obtain the resistivity at that test point. The average value of the 8 resistivities is taken as the resistivity of the positive electrode film.

[0165] In some embodiments, the resistivity of the positive electrode film can be selected from 10 Ω·cm, 11 Ω·cm, 12 Ω·cm, 13 Ω·cm, 14 Ω·cm, 15 Ω·cm, 16 Ω·cm, 17 Ω·cm, 18 Ω·cm, 19 Ω·cm, 20 Ω·cm, 21 Ω·cm, 22 Ω·cm, 23 Ω·cm, 24 Ω·cm, 25 Ω·cm, 26 Ω·cm, 27 Ω·cm, 28 Ω·cm, 29 Ω·cm, 30 Ω·cm, 31 Ω·cm, 32 Ω·cm, 32.2 Ω·cm, 33 Ω·cm, 34 Ω·cm, 35 Ω·cm, or any value between the two.

[0166] This application embodiment controls the area ratio of small particles in the positive electrode film layer, so that the resistivity of the positive electrode film layer is in a low range. This helps to reduce electron transport impedance, reduce charge and discharge polarization, thereby reducing heat generation of the positive electrode during cycling. It also helps to conduct the heat accumulated at the tab to the main body area of ​​the electrode and achieve efficient heat dissipation through the electrode surface. This reduces the probability of encapsulation failure near the current lead, improves the safety and cycle performance of the soft-pack battery cell, and enhances the safety performance of the battery device.

[0167] In some embodiments, the diaphragm includes a base membrane, ceramic layers disposed on both sides of the base membrane, and an adhesive layer disposed on at least one side of the ceramic layer away from the base membrane. The adhesive layer is a continuous layer with a porous structure and includes a vinylidene fluoride polymer.

[0168] In some embodiments, the vinylidene fluoride polymer includes vinylidene fluoride homopolymer (PVDF) and copolymers of vinylidene fluoride with other monomers, such as copolymers of vinylidene fluoride and hexafluoropropylene.

[0169] In existing technologies, aqueous PVDF is often used as the adhesive layer for separators. This adhesive layer typically exhibits an island-like structure within the separator, which is beneficial for providing gaps for cell expansion and for ease of manufacturing. However, such separator adhesive layers have low bonding area and weak adhesion. The adhesive layer of the separator in this application embodiment has a certain porous structure within its continuous structure. This porous structure allows observation of the ceramic layer disposed between the base film and the adhesive layer. It is understood that when a porous continuous layer is used as the adhesive layer, it may become blocky during electrode manufacturing or cycling due to contact with the positive or negative electrode or under pressure. The continuous layer referred to in this application does not require the adhesive layer to be continuous throughout the entire battery; rather, it refers to a continuous layer with a uniform porous structure at the microscopic level, such as when observed under a microscope, rather than an island-like structure. To accurately reflect the true morphology of the separator, sampling is preferably performed in areas of the battery where there is minimal adhesion between the separator adhesive layer and the positive or negative electrode. For example, sampling can be performed at locations on the separator where the projection extends beyond the positive or negative electrode; or sampling can be performed near the surface of the electrode assembly. Separators sampled in this way are more likely to reflect the true state of the separator.

[0170] The separator provided in this application uses a continuous layer with a porous structure as the adhesive layer, which has a larger bonding area than the island-shaped adhesive layer in the prior art, thereby making the adhesion between the separator and the positive electrode film more firm and uniform. At the same time, thanks to the porous structure in the adhesive layer, it can also achieve lithium-ion transport efficiency and reduce electrochemical heat generation.

[0171] In this embodiment, a continuous layer with a porous structure is used as an adhesive layer to improve the adhesion between the separator and the electrode while maintaining the air permeability and porosity of the separator, thereby improving the compactness of the module, reducing the interface resistance, reducing the heat generation of the pouch cell during cycling, and improving the cycle performance of the pouch cell.

[0172] In some embodiments, as shown in FIG5, the length dimension L0 of the soft-pack battery cell is 500mm-1250mm; the width dimension W0 is 100mm-150mm; and the thickness dimension H0 is 14mm-22mm.

[0173] The dimensions of the soft-pack battery cells in this application embodiment are within the above-mentioned range, which is beneficial for achieving better capacity of the battery cells and improving the overall capacity of the battery device.

[0174] In some implementations, L0 can be selected as 500mm, 510mm, 520mm, 530mm, 540mm, 550mm, 560mm, 570mm, 580mm, 590mm, 600mm, 610mm, 620mm, 630mm, 640mm, 650mm, 660mm, 670mm, 680mm, 690mm, 700mm, 710mm, 720mm, 750mm, 800mm, 850mm, 900mm, 950mm, 1000mm, 1050mm, 1100mm, 1150mm, 1200mm, 1250mm, or any value range between the two.

[0175] In some implementations, W0 can be selected as 100mm, 110mm, 120mm, 130mm, 140mm, 150mm or any value range between the two.

[0176] In some implementations, H0 can be selected as 14mm, 15mm, 16mm, 17mm, 18mm, 19mm, 20mm, 21mm, 22mm or any value range between the two.

[0177] In some implementations, the length dimension L0 of the pouch cell satisfies: 500mm≤L0≤650mm.

[0178] When the length dimension L0 of a pouch cell satisfies 500mm≤L0≤650mm, the pouch cell has a shorter length, which helps to shorten the electron transport path, reduce the internal resistance of the battery, and thus reduce the heat generation of the battery. Especially under fast charging conditions, it can reduce the uneven temperature rise and uneven current density along the length of the electrode, and improve the cycle performance of the pouch cell.

[0179] In some implementations, the length dimension L0 of the pouch cell satisfies: 900mm≤L0≤1250mm.

[0180] When the length dimension L0 of a pouch cell satisfies 900mm≤L0≤1250mm, the significantly increased cell size is more conducive to module-free integration, enabling the cell to be directly integrated into the battery device, significantly improving space utilization, thereby increasing the overall capacity of the battery device in the same volume, while reducing the number of structural components and improving the overall capacity of the battery device.

[0181] In some embodiments, referring to FIG8, the packaging bag 201 includes an encapsulation layer 223, a metal layer 222, and a protective layer 221 stacked sequentially from the inside of the battery cell to the outside of the battery cell. The metal layer 222 includes aluminum; the encapsulation layer 223 and the protective layer 221 include resin material.

[0182] In some implementations, the packaging bag is sealed by melting and bonding the sealing layers together.

[0183] In some embodiments, an encapsulation is formed between the packaging bag and the current lead by adhesive. It is understood that this adhesive may be formed by melting the encapsulation layer resin inside the packaging bag, or it may be formed together with the packaging bag and other applied adhesives.

[0184] Packaging bag materials containing the above-mentioned components have high elongation, which helps to improve the space utilization of battery cells, thereby increasing the energy density and capacity of battery cells. However, the composite material composed of aluminum and resin has poor thermal conductivity, resulting in low heat dissipation efficiency of pouch battery cells. Therefore, if the area ratio of small particles in the positive electrode film is too high, it will increase the resistivity of the positive electrode film, leading to excessive heat generation during battery cycling and exacerbating the problem of poor heat dissipation in pouch battery cells. The embodiments of this application, by using the above-mentioned packaging bag and controlling the area ratio of small particles in the positive electrode film within a suitable range, achieve high capacity, good safety and cycle performance for pouch battery cells, and high overall capacity and good safety performance for the battery device.

[0185] In some embodiments, the encapsulation layer comprises a polypropylene layer; the protective layer comprises one or more of nylon and polyethylene terephthalate (PET). In some embodiments, the encapsulation layer comprises a polypropylene (PP) layer and a modified polypropylene (PPa) layer disposed between the polypropylene (PP) layer and the metal layer; the protective layer comprises one or more of nylon and polyethylene terephthalate (PET).

[0186] In this article, modified polypropylene refers to functionalized materials that optimize the properties of ordinary polypropylene (PP) through chemical or physical means, including but not limited to grafting maleic anhydride onto the polypropylene molecular chain, introducing ethylene monomers to copolymerize with propylene, blending polypropylene with polyolefin elastomers or EPDM rubber, and adding nano-inorganic particles (such as nano-silica). Different modification methods are beneficial for specifically improving the heat-sealing properties, chemical resistance, adhesion and mechanical strength of the material.

[0187] Modified polypropylene further improves the electrolyte corrosion resistance and bonding strength of the packaging bag. This encapsulation layer helps reduce interface leakage caused by insufficient heat sealing strength. The outer protective layer has excellent mechanical properties, which can buffer mechanical impact during assembly, reduce the risk of encapsulation failure of soft-pack battery cells, improve the safety performance of soft-pack battery cells, and thus improve the reliability of battery devices.

[0188] In some embodiments, the modified polypropylene (PPa) layer comprises maleic anhydride-grafted polypropylene.

[0189] Studies have shown that the main encapsulation failure sites near the current lead are the interfacial delamination between the polypropylene layer and the metal layer under high temperatures. The carboxyl groups (—COOH) and anhydride groups (—CO—O—CO—) of maleic anhydride can chemically bond with the hydroxyl groups (—OH) or alumina (Al2O3) on the aluminum foil surface, while simultaneously maintaining molecular chain entanglement with the polypropylene matrix. This helps to further improve the peel strength between the encapsulation layer and the metal layer, reducing the probability of delamination between the encapsulation layer and the metal layer under heat flow, lowering the risk of encapsulation failure in individual pouch cells, further improving the safety performance of pouch cell pouch cells, and enhancing the reliability of the battery device.

[0190] In some embodiments, the packaging bag is heat-sealed at 180°C-220°C.

[0191] The heat sealing temperature of the packaging bag is within the above range, which helps to enhance the interfacial bonding strength, reduce the probability of delamination between the encapsulation layer and the metal layer during battery cycling, reduce the risk of encapsulation failure of soft-pack battery cells, improve the safety performance of soft-pack battery cells, and improve the reliability of battery devices.

[0192] In some embodiments, the packaging bag is heat-sealed at 200°C-210°C.

[0193] The heat sealing temperature of the packaging bag is within the above range, which helps to further enhance the bonding strength between the encapsulation layer and the metal layer, thereby reducing the probability of delamination between the encapsulation layer and the metal layer during battery cycling, reducing the risk of encapsulation failure of soft-pack battery cells, improving the safety performance of soft-pack battery cells, and thus improving the reliability of battery devices.

[0194] In some embodiments, as shown in FIG3, a thermally conductive structural adhesive 4 is provided between the support plate 11 of the housing and the soft-pack battery cell 2.

[0195] The thermally conductive structural adhesive of this application embodiment has good thermal conductivity and mechanical properties, which is beneficial for heat transfer from the soft-pack battery cell to the support plate for heat dissipation, thereby improving the cycle performance and safety performance of the soft-pack battery cell.

[0196] In some embodiments, as shown in FIG4, a thermal management component 3 is provided between the support plate 11 of the housing and the second surface 22 of the soft-pack battery cell 2. The thermal management component 3 is used to regulate the temperature of the soft-pack battery cell 2, and a thermally conductive structural adhesive 4 is provided between the thermal management component 3 and the second surface 22 of the soft-pack battery cell 2.

[0197] The heat from a single pouch battery cell can be efficiently dissipated through thermal management components, which helps to further improve the cycle performance and safety performance of the pouch battery cell.

[0198] In some embodiments, at 85°C, the thermal conductivity of the thermally conductive structural adhesive is greater than or equal to 0.4 W / (m·K), optionally 0.4 W / (m·K)-1.2 W / (m·K), and further optionally 0.8 W / (m·K)-1.2 W / (m·K).

[0199] The thermal conductivity of the thermally conductive structural adhesive at 85°C can be tested using methods known in the art. As an example, the transient hot disk method (Hot Disk) can be used, according to ISO 22007-2. A temperature probe with a self-heating function is placed under a sample disc with a diameter greater than 30 mm and a thickness greater than 2 mm. Standard weights from Hengzhong Company are used to press down on the sample disc. During the test, a constant heating power is applied to the nickel coil of the probe, causing its temperature to rise. Since the temperature coefficient of resistance (TCR) of nickel is linear (ΔR / R0 = αΔT), the heat loss can be obtained by measuring the change in resistance, thereby determining the thermal conductivity of the sample at 85°C.

[0200] In some embodiments, the thermal conductivity of the thermally conductive structural adhesive at 85°C can be selected as 0.4 W / (m·K), 0.5 W / (m·K), 0.6 W / (m·K), 0.7 W / (m·K), 0.8 W / (m·K), 0.81 W / (m·K), 0.82 W / (m·K), 0.83 W / (m·K), 0.84 W / (m·K), 0.85 W / (m·K), 0.86 W / (m·K), 0.87 W / (m·K), or 0.88 W / (m·K). The values ​​are 0.89 W / (m·K), 0.90 W / (m·K), 0.91 W / (m·K), 0.92 W / (m·K), 0.93 W / (m·K), 0.94 W / (m·K), 0.95 W / (m·K), 0.96 W / (m·K), 0.97 W / (m·K), 0.98 W / (m·K), 0.99 W / (m·K), 1.0 W / (m·K), 1.1 W / (m·K), 1.2 W / (m·K), or any range between the two.

[0201] The thermal conductivity of the thermally conductive structural adhesive is within the above range, which has good thermal conductivity and can still conduct heat stably at high temperatures. This helps reduce the probability of thermally conductive structural adhesive failure due to temperature rise, which in turn leads to the inability of heat to be transferred from the pouch cell to the thermal management component or support plate for heat dissipation in time, resulting in heat accumulation inside the cell. This is beneficial to improving the cycle performance of the pouch cell during long-term cycling.

[0202] In some embodiments, the thermal conductivity of the thermally conductive structural adhesive is 0.8 W / (m·K)-1.0 W / (m·K) at 85°C.

[0203] If the thermal conductivity of the thermally conductive structural adhesive is within the above range, it means that the thermally conductive filler content of the thermally conductive structural adhesive is moderate, which is beneficial to balancing the thermal conductivity and mechanical properties of the thermally conductive structural adhesive.

[0204] In some embodiments, the thermally conductive structural adhesive has a storage modulus of 260MPa-1000MPa at a vibration frequency of 0.1Hz at room temperature, optionally 300MPa-800MPa, and further optionally 300MPa-600MPa.

[0205] In this application, room temperature refers to 25°C.

[0206] The storage modulus of thermally conductive structural adhesive at a vibration frequency of 0.1 Hz at room temperature can be tested using methods known in the art. As an example, dynamic thermomechanical analysis (DMA, according to IPC-TM-650 2.4.24.4) was used, employing a three-point bending test mode with a sample size of 60 mm (length) × 10 mm (width) × 2 mm (thickness). A prestress of 0.5 N–1.0 N was applied before testing, with the loading frequency set to 0.1 Hz. The temperature program was used to increase the temperature from -40 °C to 80 °C at a rate of 5 °C / min, with the default environment being air (humidity ≤30%); nitrogen protection can be used in special cases. This allows the storage modulus of the thermally conductive structural adhesive at a vibration frequency of 0.1 Hz at room temperature to be obtained.

[0207] In some embodiments, the thermally conductive structural adhesive has a storage modulus at a vibration frequency of 0.1 Hz at room temperature, which can be selected as 260 MPa, 270 MPa, 280 MPa, 290 MPa, 300 MPa, 350 MPa, 400 MPa, 450 MPa, 500 MPa, 550 MPa, 600 MPa, 650 MPa, 700 MPa, 750 MPa, 800 MPa, 850 MPa, 900 MPa, 950 MPa, 1000 MPa, or any value range between the two.

[0208] At room temperature, the energy storage modulus at a vibration frequency of 0.1 Hz is within the above range. It has good mechanical properties and can reduce the probability of creep deformation or fatigue cracking of the thermally conductive structural adhesive under long-term mechanical vibration. This reduces the probability of displacement of the soft-pack battery cell and loss of its own thermal conductivity caused by the deformation of the thermally conductive structural adhesive. The thermally conductive structural adhesive can give full play to its good thermal conductivity and further improve the cycle performance of the soft-pack battery cell in the long cycle process.

[0209] In some embodiments, the glass transition temperature of the thermally conductive structural adhesive is 50°C-60°C.

[0210] The glass transition temperature (Tg) of the thermally conductive structural adhesive can be tested using methods known in the art. As an example, dynamic thermomechanical analysis (DMA, according to IPC-TM-650 2.4.24.4) is used, and the Tg is determined by monitoring changes in the mechanical properties of the material under dynamic loads. In the test, the temperature at which the loss factor (tanδ) curve reaches its peak is the glass transition temperature (Tg). In some embodiments, the glass transition temperature of the thermally conductive structural adhesive can be selected as 50°C, 51°C, 52°C, 53°C, 54°C, 55°C, 56°C, 57°C, 58°C, 59°C, 60°C, or any value between two of these ranges.

[0211] If the glass transition temperature of the thermally conductive structural adhesive is too low, when the operating temperature of the pouch cell exceeds this glass transition temperature, the energy storage modulus of the thermally conductive structural adhesive will drop sharply, causing the adhesive to transition from a glassy state to a viscoelastic state. After softening, the adhesive cannot provide sufficient mechanical holding force, and relative displacement or interfacial debonding may occur between the pouch cell and the thermal management components or support plate, reducing the thermal conductivity between the cell and the thermally conductive structural adhesive, and consequently reducing the heat dissipation efficiency of the cell. If the glass transition temperature of the thermally conductive structural adhesive is too high, at low temperatures, the adhesive remains in a glassy state, its toughness decreases, and the volume changes of the pouch cell during charging and discharging will generate stress at the interface, causing the thermally conductive structural adhesive to brittlely crack and develop fissures, resulting in a decrease in the heat dissipation efficiency of the cell.

[0212] When the glass transition temperature of the thermally conductive structural adhesive is within a suitable range, it is beneficial for the thermally conductive structural adhesive to fully exert its bonding and thermal conductivity, which is conducive to further improving the cycle performance of the soft-pack battery cells.

[0213] In some embodiments, the thermally conductive structural adhesive comprises a polyurethane resin and thermally conductive filler particles dispersed in the polyurethane resin; the thermally conductive filler particles comprise one or more of aluminum hydroxide particles and boron nitride particles.

[0214] Thermally conductive structural adhesives containing the above components exhibit good high-temperature resistance.

[0215] In some embodiments, the thermally conductive filler particles account for 20%-70% of the total mass of the thermally conductive structural adhesive, and optionally 30%-60%.

[0216] In some embodiments, based on the total mass of the thermally conductive structural adhesive, the mass percentage of the thermally conductive filler particles can be selected as 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, or any range between the two.

[0217] The thermally conductive filler particles in the thermally conductive structural adhesive are within the above-mentioned range, which is beneficial to improving the thermal conductivity of the thermally conductive structural adhesive and reducing the problem of insufficient resin content caused by excessive thermally conductive filler particles, which would result in poor energy storage modulus of the thermally conductive structural adhesive. The thermally conductive structural adhesive has good thermal conductivity, which is beneficial to improving the cycle performance of soft-pack battery cells.

[0218] In some embodiments, as shown in Figures 2, 3, and 4, the projection of the thermally conductive structural adhesive on the first surface does not overlap with the projection of the negative electrode sheet on the first surface.

[0219] After the battery cells are bonded to the thermally conductive structural adhesive, the adhesive may overflow. Once the battery cells are assembled into a battery device, the projection of the thermally conductive structural adhesive on the first surface does not overlap with the projection of the negative electrode sheet on the first surface. This reduces the probability of the relatively rigid thermally conductive structural adhesive and the electrode sheet directly compressing each other during battery cycling, lowering the probability of stress concentration on the battery electrode sheet caused by the thermally conductive structural adhesive, thereby reducing the adverse impact on the cycle performance of the pouch battery cells.

[0220] In some embodiments, as shown in Figures 2, 3, and 4, double-sided adhesive is provided between the individual soft-pack battery cells, and a gap is provided between the double-sided adhesive and the thermally conductive structural adhesive.

[0221] After the battery cells are bonded to the thermally conductive structural adhesive, excess adhesive may appear. The battery cells are then bonded together using double-sided adhesive. After assembling them into a battery device, a gap is created between the double-sided adhesive and the thermally conductive structural adhesive. This reduces the probability of the relatively rigid thermally conductive structural adhesive and the double-sided adhesive coming into contact with each other during battery cycling. This reduces stress concentration caused by the rigid thermally conductive structural adhesive on the double-sided adhesive between the battery cells, thereby minimizing any adverse impact on the cycle performance of the pouch battery cells.

[0222] In some embodiments, the positive current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer substrate and a metal layer formed on at least one surface of the polymer substrate. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0223] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer substrate and a metal layer formed on at least one surface of the polymer substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0224] In some embodiments, the negative electrode film layer includes a negative electrode active material. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, and hard carbon. However, this application is not limited to these materials, and other conventional materials that can be used as battery negative electrode active materials may also be used. These negative electrode active materials may be used alone or in combination of two or more.

[0225] In some embodiments, the negative electrode film layer may optionally include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0226] In some embodiments, the negative electrode film may optionally include a conductive agent. The conductive agent may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0227] In some embodiments, the negative electrode film may optionally include other additives, such as thickeners (e.g., sodium carboxymethyl cellulose (CMC-Na)).

[0228] The electrolyte acts as a conductor of ions between the positive and negative electrodes. This application does not impose specific restrictions on the type of electrolyte; it can be selected according to requirements. For example, the electrolyte can be liquid, gel, or entirely solid.

[0229] In some embodiments, the electrolyte is an electrolyte solution. The electrolyte solution includes an electrolyte salt and a solvent.

[0230] In some embodiments, the electrolyte salt may be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalate borate, lithium dioxalate borate, lithium difluorodioxalate phosphate, and lithium tetrafluorooxalate phosphate.

[0231] In some embodiments, the solvent may be selected from at least one of ethylene carbonate, propylene carbonate, methyl ethyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butyl carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, sulfolane, dimethyl sulfone, methyl ethyl sulfone, and diethyl sulfone.

[0232] In some embodiments, the electrolyte may optionally include additives. For example, additives may include negative electrode film-forming additives, positive electrode film-forming additives, and may also include additives that can improve certain battery performance, such as additives that improve battery overcharge performance, additives that improve battery high-temperature or low-temperature performance, etc.

[0233] In some embodiments, the battery cell also includes a separator. This application does not impose any particular limitation on the type of separator; any known porous separator with good chemical and mechanical stability can be selected.

[0234] In some embodiments, the material of the separator can be selected from at least one of glass fiber, nonwoven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.

[0235] The battery device disclosed in this application can be used in electrical devices that use the battery device as a power source or in various energy storage systems that use the battery device as an energy storage element. Besides vehicles, the battery device can also be used in, but is not limited to, mobile phones, tablets, laptops, electric toys, power tools, electric vehicles, electric cars, ships, spacecraft, etc. Electric toys can include stationary or mobile electric toys, such as game consoles, electric car toys, electric ship toys, and electric airplane toys, etc. Spacecraft can include airplanes, rockets, space shuttles, and spacecraft, etc.

[0236] Furthermore, a second aspect of this application provides an electrical device that uses a battery as a power source, the electrical device including at least one of the battery cell, battery module, or battery pack provided in this application. The battery cell, battery module, or battery pack can be used as a power source for the electrical device, or as an energy storage unit for the electrical device.

[0237] As the electrical device, a single battery cell, a battery module, or a battery pack can be selected according to its usage requirements.

[0238] Figure 9 shows an example of an electrical device. The electrical device disclosed in this application can be a gasoline-powered vehicle, a natural gas-powered vehicle, or a new energy vehicle. New energy vehicles can be pure electric vehicles, hybrid electric vehicles, or range-extended electric vehicles, etc. A battery device is installed inside the vehicle, and the battery device can be located at the bottom, front, or rear of the vehicle. The battery device can be used to power the vehicle; for example, the battery device can serve as the vehicle's operating power source. The vehicle may also include a controller and a motor. The controller is used to control the battery device to supply power to the motor, for example, for the vehicle's starting, navigation, and operating power needs. In some embodiments of this application, the battery device can not only serve as the vehicle's operating power source but also as the vehicle's drive power source, replacing or partially replacing gasoline or natural gas to provide driving power to the vehicle.

[0239] The third aspect of this application also provides an energy storage device that uses a battery device as a power source. The energy storage device can be, but is not limited to, an energy storage container, an energy storage cabinet, an energy storage power station, an energy storage battery pack, or a portable energy storage system.

[0240] Example

[0241] The following describes embodiments of this application. The embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.

[0242] Example 1

[0243] (1) Preparation of positive electrode active material

[0244] Lithium carbonate, iron phosphate, titanium dioxide, vanadium pentoxide, sucrose, glucose, and polyethylene glycol were added to deionized water (pH=7, conductivity ≤1μS / cm) and mixed in a premixing tank. The ratio of lithium carbonate to iron phosphate was such that the molar ratio of lithium to iron was 1.02:1.0. Based on the total mass of the mixed raw materials, the mass content of sucrose was 2%, the mass content of glucose was 4%, and the mass content of polyethylene glycol was 4.5%. After uniform mixing, a mixed raw material with a solid content of 38% was obtained.

[0245] Among them, the particle size Dv of lithium carbonate 50 The particle size is 7 μm and the moisture content is 0.1%; the morphology of the iron phosphate particles is spherical; both titanium dioxide and vanadium pentoxide are nanoparticles; the purity of sucrose is ≥98%; the moisture content of glucose is <0.5%; and the weight average molecular weight of polyethylene glycol is 1400.

[0246] The mixed raw materials were ground twice in a sand mill with zirconium beads added. After coarse grinding for 1 hour, fine grinding was performed. During the grinding process, the slurry temperature was controlled to be less than 40 degrees Celsius to obtain a mixed slurry. The particle size Dv50 of the solid particles in the mixed slurry was 0.5 μm. The powder was spray-dried to obtain a dried precursor powder with an inlet air temperature of 200°C. After drying, the particle size Dv50 was 65 μm.

[0247] The precursor powder was subjected to a two-stage heating sintering process in a nitrogen atmosphere to obtain the positive electrode active material: the temperature was increased from 25℃ to 460℃ at a heating rate of 2℃ / min (first heating stage), and held for 3 hours; the temperature was then increased from 460℃ to 780℃ at a heating rate of 5℃ / min (second heating stage), and held for 12 hours; the air volume in the heating stage was greater than that in the isothermal stage, with a ratio of 1.5:1, and the total air volume was 1350 cm³. 3 / h, after which the temperature is lowered; after air jet pulverization at a pulverizing pressure of 400Kpa, a lithium iron phosphate cathode active material with a particle size Dv50 of 2.0μm and a carbon material on the surface is obtained. Based on the total mass of the cathode active material, the mass content of Ti element is 1000ppm and the mass content of V element is 1000ppm.

[0248] The Dv10, Dv50, and Dv90 mentioned above refer to data obtained through the Malvern laser scattering method.

[0249] (2) Preparation of positive electrode sheet

[0250] The above-mentioned positive electrode active material (94.6% by mass), conductive agent (2.4% by mass), and binder polyvinylidene fluoride (3% by mass) were mixed in the solvent N-methylpyrrolidone and thoroughly mixed, stirred, and dispersed in a mixing tank to form a positive electrode slurry. After the stirring process, the positive electrode slurry was transported to the coating process. The mass percentages of the positive electrode active material, conductive agent, binder, and dispersant were calculated based on the total mass of solids in the positive electrode slurry. The conductive agent included conductive carbon black (1.2% by mass) and multi-walled carbon nanotubes (1.2% by mass), and the specific surface area of ​​the conductive carbon black was 80 m². 2 / g, oil absorption value of 180ml / 100g, average length of multi-walled carbon nanotubes of 20μm, specific surface area of ​​280m² 2 / g;

[0251] The positive electrode slurry was transferred and coated onto a current collector aluminum foil, dried, and then hot-pressed to obtain a positive electrode film with a resistivity of 33.5 Ω·cm, a single-sided thickness of 107.98 μm, and a compaction density of 2.32 g / cm³. 3 The positive electrode sheet. The transfer coating speed is 20 m / min.

[0252] The hot pressing process includes three hot roller pressing processes, with the hot roller pressing pressure increasing sequentially to 40 tons, 60 tons, and 80 tons. The hot roller temperature is 60℃. Before the first hot roller compaction, the electrode sheet is heated to 40℃.

[0253] The compaction density here refers to the compaction density of a single battery cell under full discharge conditions. The test method is described above.

[0254] The positive electrode sheets are slit and punched into specified shapes, and then the punched positive electrode sheets are sorted by weight using a weighing and sorting machine for stacking by a stacking machine.

[0255] (3) Preparation of negative electrode sheet

[0256] Natural graphite, conductive carbon black, styrene-butadiene rubber (SBR) binder, and sodium carboxymethyl cellulose (CMC) thickener are mixed evenly in a weight ratio of 95:1:2:2 and deionized water is added. After stirring and dispersing, a negative electrode slurry is obtained. The negative electrode slurry is coated on a copper foil substrate, and after drying, compaction, slitting, and sheet forming, a negative electrode sheet is obtained.

[0257] The negative electrode sheets are slit and punched into specified shapes, and then the punched negative electrode sheets are sorted by weight using a weighing and sorting machine for stacking by a stacking machine.

[0258] (4) Diaphragm

[0259] Polyvinylidene fluoride (PVDF) was dissolved in N-methylpyrrolidone (NMP) and stirred until homogeneous. Polyethylene glycol (PEG) was then added as a pore-forming agent and thoroughly mixed to obtain an adhesive layer solution. This adhesive layer solution was applied to a base film with ceramic layers on both sides. After pre-evaporation at 80°C and drying at 110°C, the film was immersed in deionized water to dissolve the PEG, resulting in a membrane with porous adhesive layers on both sides. The base film thickness was 8 μm, the ceramic layer thickness on one side was 3 μm, and the adhesive layer thickness on one side was 1 μm.

[0260] (5) Electrolyte

[0261] In an argon atmosphere glove box (H2O < 0.1 ppm, O2 < 0.1 ppm), organic solvents dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), and ethylene carbonate (EC) are mixed evenly.

[0262] Lithium hexafluorophosphate was then added and dissolved in an organic solvent to achieve a concentration of 1.05 mol / L. Ethylene carbonate (VC) was then added and stirred until homogeneous to obtain the electrolyte of Example 1.

[0263] Based on the total mass of the electrolyte, the mass content of dimethyl carbonate is 26%, the mass content of methyl ethyl carbonate is 43.3%, the mass content of ethylene carbonate is 17.3%, and the mass content of vinylene carbonate is 0.9%.

[0264] (6) Preparation of soft-pack battery cells

[0265] The positive electrode, separator, and negative electrode are stacked in sequence using a stacking machine. The separator must effectively isolate the positive and negative electrodes to obtain a stacked battery cell. The stacked battery cell is then coated with adhesive to ensure tight containment. The coated stacked battery cell is placed in a packaging bag made of aluminum-plastic film, a soft-pack material composed of a polypropylene encapsulation layer, an aluminum foil metal layer, and a nylon protective layer. The aluminum-plastic film packaging bag is shaped and trimmed using a punching and forming machine to achieve the desired shape and size. The aluminum-plastic film is then heat-sealed at 195℃, ensuring a sealing tensile strength ≥25N / 8mm. The battery undergoes vacuum baking, settling, electrolyte injection, and sealing. Finally, the soft-pack battery is subjected to hot and cold pressing operations: hot pressing at 45℃ for 2 minutes and a pressure of 90kg / cm². 2 The cold pressing temperature was 25℃, the time was 2 minutes, and the pressure was 90 kg / cm². 2 Finally, after processes such as formation, vacuum degassing, and edge trimming, a pouch cell is obtained. The pouch cell has dimensions of 630mm in length, 130mm in width, and 20mm in thickness.

[0266] (7) Preparation of thermally conductive structural adhesive

[0267] Preparation of Component A: Polyether-modified polyol (Wanhua Chemical, grade C2004), castor oil-modified polyol (Wanhua Chemical, grade C1030D), chain extender butanediol, and thermally conductive filler aluminum hydroxide (Foshan Jingge, JAZ-176) were mixed in a mass ratio of 12:20:4:58 to obtain the first raw material. The first raw material was added to the first stirred tank and heated, stirred, and vacuumed to remove water. The water removal temperature was 120℃, the vacuum degree was -0.08MPa, the water removal time was 2h, and the rotation speed was 10rpm. After stirring and removing water, the mixture was cooled to room temperature. Then, 4 parts by mass of molecular sieve (Luoyang Jianlong, JLH-03-B), 1.5 parts by mass of silica (Evonik, grade R974), 0.2 parts by mass of catalyst dibutyltin dilaurate, and 0.3 parts by mass of yellow paste (Shanghai Jiasheng) were added to the first stirred tank and stirred and mixed evenly under vacuum to obtain Component A.

[0268] Preparation of Component B: 19 parts by weight of polyester polyol (Shanghai Jingri, DA21) were added to the second stirred tank and heated to 115℃ for dehydration for 2.5 h; then cooled to below 60℃, and 20 parts by weight of isocyanate (Wanhua Chemical, CDMDI-100L) were added. Under nitrogen protection, the mixture was heated to 65℃ at 30 rpm and stirred for 2.5 h. After the reaction, the second raw material (isocyanate prepolymer) was obtained; then, in the second stirred tank, [the following was added]... 46 parts by weight of thermally conductive filler aluminum hydroxide (Foshan Jingge, JAZ-176), 4 parts by weight of plasticizer dinonyl phthalate (Ningbo Taiying), 7 parts by weight of hydrophobic silica powder (Shenzhen Jinhaohui, GL15P3), 2.7 parts by weight of fumed silica (Jiangsu Haoneng Chemical, HN-200), 1 part by weight of molecular sieve (Luoyang Jianlong, JLH-03-B), and 0.3 parts by weight of blue paste (Shanghai Jiasheng) were mixed evenly under vacuum at 25°C for 2 hours to obtain component B.

[0269] A high-performance two-component polyurethane thermally conductive structural adhesive can be obtained by mixing component A and component B at a volume ratio of 1:1 and curing at room temperature for 7 days.

[0270] The thermally conductive structural adhesive has a thermal conductivity of 0.8 W / (m·K) at 85℃, a storage modulus of 500 MPa at room temperature and a vibration frequency of 0.1 Hz, and a glass transition temperature of 55℃.

[0271] (7) Preparation of battery device

[0272] Multiple pouch battery cells prepared above are sequentially bonded to the thermal management component along the first direction using the thermally conductive structural adhesive prepared above. After bonding, the component is moved into the housing. The housing includes a support plate, a frame, and a connecting beam to obtain the battery device. During the bonding process, the thermally conductive structural adhesive will overflow. After overflow, the projection of the thermally conductive structural adhesive on the first surface does not overlap with the projection of the negative electrode sheet in the pouch battery cell on the first surface.

[0273] Example 2

[0274] The preparation method of Example 2 is basically the same as that of Example 1, except that the preparation method of the positive electrode active material is adjusted, as follows:

[0275] First, a precursor solution was prepared under argon protection by mixing FeSO4·7H2O, LiOH·H2O, and H3PO4 in deionized water, and adding 0.5wt% ascorbic acid as an antioxidant. Then, the pH was adjusted to 5.0, and 0.1mol / L citric acid was added as a grain growth inhibitor and 1wt% PEG-4000 as a dispersant. The mixed solution was transferred to a high-pressure reactor and reacted at 180℃ for 6 hours. After centrifugation and washing, the reaction product was vacuum dried at 80℃ and finally annealed at 350℃ in an argon atmosphere for 2 hours to obtain lithium iron phosphate material with an average particle size of 160nm.

[0276] The lithium iron phosphate material prepared above was mixed with the positive electrode active material of Example 1 at a mass ratio of 10:90 to obtain the positive electrode active material of Example 2.

[0277] The positive electrode slurry from Example 2 was transferred and coated onto the current collector aluminum foil and dried. By adjusting the pressure, rolling speed, roll gap, holding time, number of rolling passes, and controlling the coating density during the hot pressing process, a compacted density of 2.32 g / cm³ was obtained after hot pressing. 3 The positive electrode sheet. The compaction density here refers to the compaction density of the battery cell under full discharge conditions; the test method is described above.

[0278] Example 3

[0279] The preparation method of Example 3 is basically the same as that of Example 1, except that the preparation method of the positive electrode active material is adjusted. The positive electrode active material of Example 3 is obtained by increasing the sintering temperature of the second heating stage and reducing the pulverizing gas pressure.

[0280] The positive electrode slurry from Example 3 was transferred and coated onto the current collector aluminum foil and dried. By adjusting the pressure, rolling speed, roll gap, holding time, number of rolling cycles, and controlling the coating density during the hot pressing process, a compacted density of 2.32 g / cm³ was obtained after hot pressing. 3 The positive electrode sheet. The compaction density here refers to the compaction density of the battery cell under full discharge conditions; the test method is described above.

[0281] Example 4

[0282] The preparation method of Example 4 is basically the same as that of Example 1, except that the preparation method of the positive electrode active material is adjusted as follows: the carbon source is changed from glucose and polyethylene glycol to phenolic resin, and the sintering temperature of the second heating stage is adjusted to 800°C to obtain the positive electrode active material of Example 4.

[0283] The positive electrode slurry from Example 4 was transferred and coated onto the current collector aluminum foil and dried. By adjusting the pressure, rolling speed, roll gap, holding time, number of rolling passes, and controlling the coating density during the hot pressing process, a compacted density of 2.32 g / cm³ was obtained after hot pressing. 3 The positive electrode sheet. The compaction density here refers to the compaction density of the battery cell under full discharge conditions; the test method is described above.

[0284] Example 5

[0285] The preparation method of Example 5 is basically the same as that of Example 1, except that the preparation method of the positive electrode sheet is adjusted, as follows:

[0286] The positive electrode slurry from Example 1 was transferred and coated onto a current collector aluminum foil and dried. By adjusting the pressure, rolling speed, roll gap, holding time, number of rolling passes, and controlling the coating density in the hot pressing process, a positive electrode sheet with a single-sided thickness of 119.99 μm was obtained through hot pressing; the compaction density of the positive electrode sheet was 2.32 g / cm³. 3 The compaction density here refers to the compaction density of a single battery cell under full discharge conditions; the testing method is described above. Keeping the number of layers in the stack constant, the thickness of the pouch cell is adaptively adjusted according to the thickness of the positive electrode film.

[0287] Example 6

[0288] The preparation method of Example 6 is basically the same as that of Example 1, except that the preparation method of the positive electrode sheet is adjusted, as follows:

[0289] The positive electrode slurry from Example 1 was transferred and coated onto a current collector aluminum foil and dried. By adjusting the pressure, rolling speed, roll gap, holding time, number of rolling passes, and controlling the coating density in the hot pressing process, a positive electrode sheet with a single-sided thickness of 70.22 μm was obtained; the compaction density of the positive electrode sheet was 2.32 g / cm³. 3 The compaction density here refers to the compaction density of a single battery cell under full discharge conditions; the testing method is described above. Keeping the number of layers in the stack constant, the thickness of the pouch cell is adaptively adjusted according to the thickness of the positive electrode film.

[0290] Example 7

[0291] The preparation method of Example 7 is basically the same as that of Example 1, except that the preparation method of the positive electrode sheet is adjusted, specifically as follows:

[0292] The above-mentioned positive electrode active material (94.6% by mass), conductive agent (2.4% by mass), and binder polyvinylidene fluoride (3% by mass) were mixed in the solvent N-methylpyrrolidone and thoroughly mixed, stirred, and dispersed in a mixing tank to form a positive electrode slurry. After the stirring process, the positive electrode slurry was transported to the coating process. The mass percentages of the positive electrode active material, conductive agent, binder, and dispersant were calculated based on the total mass of solids in the positive electrode slurry. The conductive agent included conductive carbon black (0.9% by mass) and multi-walled carbon nanotubes (1.5% by mass), and the specific surface area of ​​the conductive carbon black was 80 m². 2 / g, oil absorption value of 180ml / 100g, average length of multi-walled carbon nanotubes of 20μm, specific surface area of ​​280m² 2 / g.

[0293] The preparation methods of Examples 8-14 are basically the same as those of Example 1, except that the preparation methods of components A and B in the thermally conductive structural adhesive are adjusted, as shown in Table 4.

[0294] Comparative Example 1

[0295] The preparation method of Comparative Example 1 is basically the same as that of Example 1, except that the preparation method of the positive electrode active material is adjusted, as follows:

[0296] First, a precursor solution was prepared under argon protection by mixing FeSO4·7H2O, LiOH·H2O, and H3PO4 in deionized water, and adding 0.5wt% ascorbic acid as an antioxidant. Then, the pH was adjusted to 5.0, and 0.1mol / L citric acid was added as a grain growth inhibitor and 1wt% PEG-4000 as a dispersant. The mixed solution was transferred to a high-pressure reactor and reacted at 180℃ for 6 hours. After centrifugation and washing, the reaction product was vacuum dried at 80℃ and finally annealed at 350℃ in an argon atmosphere for 2 hours to obtain lithium iron phosphate material with an average particle size of 160nm.

[0297] The lithium iron phosphate material prepared above was mixed with the positive electrode active material of Example 1 at a mass ratio of 20:80 to obtain the positive electrode active material of Comparative Example 1.

[0298] The positive electrode slurry of Comparative Example 1 was transferred and coated onto the current collector aluminum foil and dried. By adjusting the pressure, rolling speed, roll gap, holding time, and number of rolling cycles in the hot pressing process, and controlling the coating density, a compacted density of 2.32 g / cm³ was obtained after hot pressing. 3 The positive electrode sheet. The compaction density here refers to the compaction density of the battery cell under full discharge conditions; the test method is described above.

[0299] Test method:

[0300] 1. Probability of encapsulation failure of individual pouch cells

[0301] At 25°C, the pouch cell in the battery device is charged to 3.65V at a 2C charging rate, which is equal to the nominal capacity of the individual pouch cells. Then, it is charged at a constant voltage of 3.65V to 0.05C. After charging is completed, the charging circuit of the battery device is disconnected and left to stand for 10 minutes. Then, the pouch cell is discharged to 2.5V at a 2C discharging rate, which is equal to the nominal capacity of the individual pouch cells. After standing for 10 minutes, one charge-discharge cycle is recorded. The cycle is paused when the number of cycles reaches 1300. The individual pouch cells in the battery device are disassembled. When misalignment and peeling occur between the encapsulation layer and the metal layer in the packaging bag near the current lead, it is considered that the pouch cell has experienced encapsulation failure. Ten pouch cells are observed simultaneously in each set of embodiments or comparative examples, and the probability of encapsulation failure is calculated.

[0302] 2. Number of cycles corresponding to 85% capacity decay

[0303] At 25°C, the battery pack cells in the device are charged to 3.65V at a charging rate of 0.5C, which is equivalent to the nominal capacity of the individual cells. Then, they are charged at a constant voltage of 3.65V to 0.05C. After charging is complete, the charging circuit of the battery pack is disconnected and left to stand for 10 minutes. Then, the battery pack cells are discharged to 2.5V at a discharge rate of 1C, which is equivalent to the nominal capacity of the individual cells. After standing for 10 minutes, one charge-discharge cycle is counted as one cycle. The test is stopped when the capacity of the battery pack is reduced to 85% of the nominal capacity. This number of cycles is recorded as the number of cycles corresponding to the capacity reduction to 85%.

[0304] 3. Thermal conductivity test of thermally conductive structural adhesive.

[0305] At 25°C, the battery pack cells in the battery device were charged to 3.65V at a 2C charging rate, equal to the nominal capacity of each cell. Then, they were charged at a constant voltage of 3.65V to 0.05C. After charging, the charging circuit was disconnected, and the battery was allowed to stand for 10 minutes. Then, the battery was discharged to 2.5V at a 2C discharging rate, equal to the nominal capacity of each cell, and allowed to stand for 10 minutes. This one charge-discharge cycle constituted one cycle. The cycle count was recorded after 300 cycles. Infrared thermal imaging was used to record the highest surface temperature of each cell in each embodiment during the cycle, in °C. As shown in Table 4, using the highest temperature of Example 2 as a benchmark, the percentage of the highest temperatures of Examples 1 and 8-14 compared to the highest temperature of Example 2 was calculated. The lower the percentage, the better the thermal conductivity of the thermally conductive structural adhesive used in that embodiment.

[0306] Test results:

[0307] Table 1

[0308] As can be seen from the comparison of the embodiments and comparative examples, the embodiments of this application integrate and assemble lithium transition metal phosphate soft-pack battery cells into a housing using a module-free integration method. When the area ratio of particles with a diameter greater than or equal to 50 nm and less than or equal to 250 nm in the cross-section of the positive electrode film along the thickness direction of the electrode sheet is 8%-25%, the soft-pack battery cell not only has a high capacity, but also further improves the safety performance of the soft-pack battery cell.

[0309] Table 2

[0310] As can be seen from the comparison between Example 2 and Examples 1, 3 and 4, when the area ratio of particles with a diameter greater than or equal to 50 nm and less than or equal to 250 nm in the cross-section of the positive electrode film along the thickness direction of the electrode sheet is 8%-20%, it is beneficial to improve the cycle performance of the soft-pack battery cell while maintaining high capacity.

[0311] As can be seen from the comparison between Examples 1, 5, and 6, the single-sided thickness of the positive electrode film is 90μm-120μm, which is beneficial to further improve the capacity of the soft-pack battery cell.

[0312] Table 3

[0313] As can be seen from the comparison between Examples 1 and 7, when the total area of ​​the conductive agent agglomeration region is 0.5%-2.0% based on the total area of ​​the cross-section of the positive electrode film along the thickness direction of the electrode sheet, it is beneficial to further improve the cycle performance of the soft-pack battery cell.

[0314] Table 4

[0315] As can be seen from the comparison between Examples 8 and Examples 1 and 9, when the thermal conductivity of the thermally conductive structural adhesive is 0.8 W / (m·K)-1.2 W / (m·K) at 85°C, it is beneficial to improve the thermal conductivity of the thermally conductive structural adhesive and reduce the temperature rise rate of the battery.

[0316] As can be seen from the comparison of Examples 10-12 and Examples 13 and 14, when the energy storage modulus of the thermally conductive structural adhesive is 300MPa-800MPa at a vibration frequency of 0.1Hz at room temperature, it is beneficial to improve the thermal conductivity of the thermally conductive structural adhesive and reduce the temperature rise rate of the battery.

[0317] It should be noted that this application is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this application are included in the technical scope of this application. Furthermore, various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing by combining some of the constituent elements of the embodiments, without departing from the spirit of this application, are also included in the scope of this application.

Claims

1. A battery device, characterized by, include: The housing includes a support plate and a frame surrounding the outer periphery of the support plate, wherein the support plate is fixedly connected to the frame. Multiple pouch battery cells are stacked and housed within a housing in a first direction; the rated capacity of each pouch battery cell is greater than or equal to 50Ah and less than or equal to 300Ah; the surface of each pouch battery cell includes a first surface and a second surface, the area of ​​the first surface being greater than the area of ​​the second surface; the first surfaces of the multiple pouch battery cells are arranged opposite each other along the first direction; and the support plate is arranged opposite to the second surfaces of the multiple pouch battery cells along a second direction. The housing is provided with at least one connecting beam extending along a third direction. The connecting beam is fixedly connected to the support plate and / or the frame. At least one soft-pack battery cell abuts against the connecting beam along the first direction. The first direction, the second direction, and the third direction are perpendicular to each other. The soft-pack battery cell includes a packaging bag, an electrode assembly, and a current lead. The electrode assembly is housed inside the packaging bag. One end of the current lead is connected to the electrode assembly, and the other end of the current lead is located outside the packaging bag. The current lead and the packaging bag are encapsulated and connected. The electrode assembly includes a positive electrode, a negative electrode, and a separator disposed between the positive and negative electrode. The positive electrode includes a positive current collector and a positive electrode film disposed on at least one side of the positive current collector. The positive electrode film includes a positive active material, which includes lithium transition metal phosphate particles with carbon material disposed on at least a portion of their surface. In the cross-section of the positive electrode film along the thickness direction of the electrode, the area ratio of particles with a diameter greater than or equal to 50 nm and less than or equal to 250 nm is 8%-25%.

2. The battery device of claim 1, wherein The rated capacity of the soft-pack battery cell is greater than or equal to 100Ah and less than or equal to 200Ah.

3. The battery device according to claim 1 or 2, characterized by In the cross-section of the positive electrode film layer along the thickness direction of the electrode sheet, the area ratio of particles with a diameter greater than or equal to 50 nm and less than or equal to 250 nm is 8%-20%.

4. The battery device according to any one of claims 1 to 3, characterized by, In the cumulative distribution curve of graphitization degree C obtained by laser microscopy confocal Raman spectroscopy in instrument scanning mode, the median C of the graphitization degree is... 50 The value is 1.00-1.20; where the degree of graphitization C is I. G / I D I G This indicates that the Raman spectrum is at 1580±100 cm⁻¹ -1 The intensity of peak G at I D This indicates that the Raman spectrum is at 1350±100 cm⁻¹ -1 The intensity of peak D at that location.

5. The battery device according to any one of claims 1 to 4, characterized by, The positive electrode film layer further includes a conductive agent, which includes carbon nanotubes. The carbon nanotubes include one or more of single-walled carbon nanotubes, few-walled carbon nanotubes, and multi-walled carbon nanotubes. Based on the mass of the positive electrode film layer, the mass content of carbon nanotubes is 0.05%-2.5%.

6. The battery device of claim 5, wherein The conductive agent also includes conductive carbon black, and the mass content of conductive carbon black is 0.05%-2.5% based on the mass of the positive electrode film.

7. The battery device according to claim 5 or 6, characterized by Based on the total area of ​​the cross-section of the positive electrode film along the thickness direction of the electrode sheet, the total area ratio of the agglomeration region of the conductive agent is 0.5%-2.5%, which can be selected as 0.5%-2%; the agglomeration region of the conductive agent includes carbon nanotubes and conductive carbon black.

8. The battery device according to any one of claims 1 to 7, characterized by, The thickness of the positive electrode film on one side is 70μm-120μm.

9. The battery device according to any one of claims 1 to 8, characterized by, The thickness of the positive electrode film on one side is 90μm-120μm.

10. The battery device according to any one of claims 1-9, wherein, The thickness of the positive electrode film on one side is 100μm-120μm.

11. The battery device of any one of claims 1-10, wherein, The soft package battery monomer in full discharge state, the compaction density of the positive pole piece is 2.3g / cm 3 -2.6g / cm 3 .

12. The battery device of any one of claims 1-11, wherein, The resistivity of the positive electrode film is 10 Ω·cm - 35 Ω·cm.

13. The battery device of any one of claims 1-12, wherein, The diaphragm includes a base membrane, ceramic layers disposed on both sides of the base membrane, and an adhesive layer disposed on at least one side of the ceramic layer away from the base membrane. The adhesive layer is a continuous layer with a porous structure and includes a vinylidene fluoride polymer.

14. The battery device of any one of claims 1-13, wherein, The length L0 of the soft-pack battery cell is 500mm-1250mm; the width W0 is 100mm-150mm; and the thickness H0 is 14mm-22mm.

15. The battery device of any one of claims 1-14, wherein, The packaging bag includes an encapsulation layer, a metal layer, and a protective layer stacked sequentially from the inside of the battery cell to the outside of the battery cell. The metal layer includes aluminum; the encapsulation layer and the protective layer include resin materials.

16. The battery device of claim 15, wherein, The encapsulation layer includes a polypropylene (PP) layer, and optionally, the encapsulation layer includes a polypropylene (PP) layer and a modified polypropylene (PPa) layer disposed between the polypropylene (PP) layer and the metal layer; the protective layer includes one or more of nylon and polyethylene terephthalate (PET).

17. The battery device of any one of claims 1-16, wherein, The modified polypropylene (PPa) layer comprises maleic anhydride-grafted polypropylene.

18. The battery device of claim 16, wherein, The packaging bag is heat-sealed at 180℃-220℃, with a possible temperature of 200℃-210℃.

19. The battery device of any one of claims 1-18, wherein, A thermally conductive structural adhesive is provided between the support plate of the housing and the individual soft-pack battery cells; and / or A thermal management component is provided between the support plate of the housing and the second surface of the soft-pack battery cell. The thermal management component is used to regulate the temperature of the soft-pack battery cell. A thermally conductive structural adhesive is provided between the thermal management component and the second surface of the soft-pack battery cell.

20. The battery device of claim 19, wherein, At 85°C, the thermal conductivity of the thermally conductive structural adhesive is greater than or equal to 0.4 W / (m·K), which can be selected as 0.4 W / (m·K)-1.2 W / (m·K), and more preferably 0.8 W / (m·K)-1.2 W / (m·K).

21. The battery device of claim 19 or 20, wherein, The thermally conductive structural adhesive has a storage modulus of 260MPa-1000MPa at a vibration frequency of 0.1Hz at room temperature, which can be selected as 300MPa-800MPa, and further selected as 300MPa-600MPa.

22. The battery device of any one of claims 19-21, wherein, The glass transition temperature of the thermally conductive structural adhesive is 50℃-60℃.

23. The battery device of any one of claims 19-22, wherein, The thermally conductive structural adhesive comprises polyurethane resin and thermally conductive filler particles dispersed in the polyurethane resin; the thermally conductive filler particles comprise one or more of aluminum hydroxide particles and boron nitride particles.

24. The battery device of claim 23, wherein, Based on the total mass of the thermally conductive structural adhesive, the mass percentage of the thermally conductive filler particles is 20%-70%, optionally 45%-65%.

25. The battery device of any one of claims 19-24, wherein, The projection of the thermally conductive structural adhesive on the first surface does not overlap with the projection of the negative electrode sheet on the first surface.

26. The battery device of any one of claims 1-25, wherein, At least some of the pouch cell units are provided with double-sided adhesive, and a gap is provided between the double-sided adhesive and the thermally conductive structural adhesive.

27. An electrical device, comprising: The electrical device includes a battery device as described in any one of claims 1-26, the battery device being used to provide electrical energy.

28. An energy storage device, comprising: The energy storage device includes a battery device as described in any one of claims 1-26, the battery device being used to store electrical energy.