Battery device, electric device, and energy storage device

By integrating modules without modules and optimizing the positive electrode film design, combined with the use of thermally conductive structural adhesive, the heat dissipation problem of soft-pack battery cells during high-density integration was solved, improving the capacity and safety of the battery device and achieving good thermal management and cycle performance.

WO2026237159A1PCT designated stage Publication Date: 2026-11-19CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2025/107794
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-12
Filing Date
2025-07-09
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

When pouch cells are integrated at high density, their heat dissipation capacity is poor, leading to heat accumulation, uneven temperature, safety hazards, and encapsulation failure, which affects the safety and reliability of the battery device.

Method used

The module-free integration method uses lithium transition metal phosphate soft-pack battery cells, combined with ceramic layer separators on both sides and a porous separator. The proportion of large particles in the positive electrode film is controlled to increase the stiffness and adhesion of the separator, improve the density of the electrode assembly, reduce the risk of short circuit, and optimize heat dissipation through thermally conductive structural adhesive and thermal management components.

Benefits of technology

It improves the overall capacity and safety performance of the battery device, reduces the probability of encapsulation failure, and improves the battery's cycle performance and thermal management efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2025107794_19112026_PF_FP_ABST
    Figure CN2025107794_19112026_PF_FP_ABST
Patent Text Reader

Abstract

The present application provides a battery device, an electric device, and an energy storage device. The battery device comprises: a case, the case comprising a support plate and a frame; and a plurality of pouch battery cells, each pouch battery cell having a rated capacity greater than or equal to 50 Ah and less than or equal to 300 Ah. At least one connecting beam is disposed in the case; the pouch battery cells abut against the connecting beam; each pouch battery cell comprises a packaging bag, an electrode assembly and a current lead-out member; the electrode assembly comprises a positive electrode film layer, and the positive electrode film layer comprises lithium-containing transition metal phosphate particles having a carbon material disposed on at least part of the surfaces thereof. In a cross section of the positive electrode film layer in the thickness direction of an electrode sheet, the area ratio of particles having a particle size greater than or equal to 1 µm is 12% to 40%. A separator comprises a base film, a ceramic layer, and a bonding layer disposed on the side, away from the base film, of the ceramic layer on at least the side close to a positive electrode sheet. The bonding layer is a continuous layer of a porous structure, and the bonding layer comprises a vinylidene fluoride polymer.
Need to check novelty before this filing date? Find Prior Art

Description

Battery devices, electrical devices and energy storage devices

[0001] Cross-references

[0002] This application claims priority to international patent application PCT / CN2025 / 094369, filed on May 12, 2025, entitled “Battery cell, battery device, power supply device and energy storage device”, the entire contents of which are incorporated herein by reference. Technical Field

[0003] This application relates to the field of battery technology, and in particular to a battery device, an electrical device, and an energy storage device. Background Technology

[0004] In recent years, the new energy industry has developed rapidly. As a core component of electric vehicles and energy storage systems, the performance of battery cells directly affects the range and safety of electrical devices. To meet market demand for high-capacity batteries, pouch cells have been widely used in the battery field due to their advantages such as light weight, flexible design, and high energy density. By optimizing the arrangement of multiple pouch cells, the integration of the battery system can be further improved, achieving a compact structure, thereby enhancing the overall energy density and range.

[0005] However, due to their soft-pack packaging, individual pouch cells have poor heat dissipation capabilities, easily accumulating heat during charging and discharging, leading to uneven temperature distribution. When multiple pouch cells are integrated at high density, the heat dissipation space is further limited, making it difficult to effectively dissipate heat. This can cause localized overheating, and even lead to safety hazards such as encapsulation failure and electrolyte leakage. In severe cases, it can even cause thermal runaway, deteriorating the safety and reliability of the battery device. Therefore, how to improve the safety performance of battery devices while increasing their capacity has become a key challenge that urgently needs to be overcome in the current battery technology field. Summary of the Invention

[0006] This application is made in view of the above-mentioned problems, and its purpose is to provide a battery device with high capacity and good safety performance.

[0007] This application provides a battery device, including a housing, a support plate, and a frame surrounding the outer periphery of the support plate, the support plate being fixedly connected to the frame; a plurality of pouch battery cells stacked in a first direction and housed within the housing; each pouch battery cell having a rated capacity greater than or equal to 50 Ah and less than or equal to 300 Ah; each pouch battery cell having a surface including a first surface and a second surface, the area of ​​the first surface being greater than the area of ​​the second surface, the first surfaces of the plurality of pouch battery cells being disposed opposite each other along the first direction, and the support plate being disposed opposite to the second surfaces of the plurality of pouch battery cells along a second direction; at least one connecting beam extending in a third direction is provided within the housing, the connecting beam being fixedly connected to the support plate and / or the frame, at least one pouch battery cell abutting against the connecting beam along the first direction, the first direction, the second direction, and the third direction being perpendicular to each other; wherein, each pouch battery cell includes The package includes a packaging bag, an electrode assembly, and a current lead. The electrode assembly is housed within the packaging bag. One end of the current lead is connected to the electrode assembly, and the other end of the current lead is located outside the packaging bag. The current lead and the packaging bag are sealed together. The electrode assembly includes a positive electrode, a negative electrode, and a separator disposed between the positive and negative electrode. The positive electrode includes a positive current collector and a positive electrode film layer disposed on at least one side of the positive current collector. The positive electrode film layer includes a positive active material, which includes lithium transition metal phosphate particles with carbon material disposed on at least a portion of its surface. In the cross-section of the positive electrode film layer along the thickness direction of the electrode, the area ratio of particles with a diameter greater than or equal to 1 μm is 12%-40%. The separator includes a base film, ceramic layers disposed on both sides of the base film, and an adhesive layer disposed on the side of the ceramic layer away from the base film, at least near the positive electrode. The adhesive layer is a continuous porous layer and includes a vinylidene fluoride polymer.

[0008] The enclosure is supported by a support plate and a frame set on the outer periphery of the support plate, which helps to reduce the weight of the enclosure in the battery device and achieve lightweighting. However, it also weakens the stability of the battery device. At least one connecting beam extending along a third direction is provided in the enclosure. The connecting beam abuts against the battery cell along the first direction and provides support force to the battery cell. This can improve the rigidity of the battery device and improve the structural stability of the battery device while maintaining its lightweight.

[0009] Soft-pack batteries have low mechanical strength and poor resistance to internal pressure. Furthermore, after the soft-pack battery cells are integrated with the casing in a module-free design, there are no modules separating a large number of battery cells. The pollution caused by the failure of the encapsulation of a single battery cell is far greater than that of a traditional module. Therefore, lithium transition metal phosphate systems, which have high safety and relatively low gas production, are particularly suitable for soft-pack batteries.

[0010] However, lithium-containing transition metal phosphates are limited by specific capacity, requiring increased compaction to improve capacity and overcome the energy density bottleneck. The applicant has discovered that a certain proportion of particle size distribution is beneficial for improving the compaction density of the positive electrode film, achieving a rated capacity of greater than or equal to 50 Ah and less than or equal to 300 Ah for each pouch cell, ensuring a considerable overall capacity for the battery device. Specifically, when the area ratio of particles with a diameter greater than or equal to 1 μm in the cross-section along the electrode thickness direction of the positive electrode film is less than 12%, insufficient particle size distribution will significantly limit the potential for increasing compaction density, thus failing to meet the design requirements for the capacity of the pouch cell. The applicant also discovered that when the area of ​​particles with a diameter greater than or equal to 1 μm in the cross-section of the positive electrode film along the thickness direction of the electrode sheet is greater than 50%, the excessive large particles will cause a severe rebound phenomenon in the positive electrode film, leading to SEI film damage and film layer cracking. This can easily cause misalignment between the positive and negative electrode sheets and the separator, increasing the risk of local short circuit in the battery. Consequently, it can lead to an increase in local current density and temperature, accelerate electrolyte decomposition, and increase gas production, thereby exacerbating the probability of encapsulation failure near the current lead-out components.

[0011] This application improves the battery capacity by using lithium transition metal phosphate (LiMT) pouch cell integrated with a module-free approach. It further utilizes a separator with ceramic layers on both sides to increase separator stiffness. Simultaneously, it employs a continuous porous separator with a larger bonding area and stronger adhesion to enhance the bonding between the separator and the positive electrode, improving the density and stiffness of the internal electrode assembly. This compensates for the weak external binding force of the electrode assembly and reduces the risk of horizontal misalignment due to mutual compression of the positive and negative electrode sheets in the thickness direction during rebound. Furthermore, by controlling the area ratio of large-diameter LiMT particles in the positive electrode film to within 12%-40%, it improves the particle size distribution of the film and reduces rebound phenomena caused by excessive large particles, lowering the risk of positive and negative electrode overlap and subsequent short circuits. It also reduces the amount of gas generated by electrolyte decomposition at high temperatures, thereby reducing the probability of encapsulation failure near the current leads and improving the safety performance of the pouch cell. The embodiments of this application improve the overall capacity and safety performance of the battery device through a module-free integration method and the synergistic design of the soft-pack battery cell, positive electrode plate and separator.

[0012] In any embodiment, the rated capacity of each of the pouch cell is greater than or equal to 100 Ah and less than or equal to 200 Ah.

[0013] The rated capacity of each of the aforementioned pouch cell is within the above-mentioned range, which is beneficial to improving the overall capacity of the battery device.

[0014] In any embodiment, in the cross-section of the positive electrode film layer along the thickness direction of the electrode sheet, the area of ​​particles with a particle size of 1μm-5μm accounts for 12%-37%.

[0015] When the area ratio of particles with a diameter of 1μm-5μm in the cross-section of the positive electrode film along the thickness direction of the electrode sheet is within the above range, it is beneficial for the soft-pack battery cell to maintain high capacity while further improving the electrode rebound phenomenon caused by stress concentration of large particles in the electrode sheet. This reduces the probability of contact and short circuit between the negative electrode film layer and the positive electrode film layer in the electrode sheet, reduces the amount of gas generated by electrolyte decomposition at high temperature, thereby reducing the probability of encapsulation failure near the current lead-out component, improving the cycle performance of the soft-pack battery cell, and the battery device with this soft-pack battery cell has good safety performance and high overall capacity.

[0016] In any embodiment, in the cross-section of the positive electrode film along the electrode thickness direction, the median L of the sphericity distribution curve of particles with a diameter greater than or equal to 1 μm is... A50 It is 0.6-0.8.

[0017] The median sphericity of particles with a diameter of 1 μm or greater is within the above range. Larger particles have better sphericity, reducing particle bridging caused by irregular particle shape, and reducing stress concentration exacerbated by the irregularity of large particles. This reduces the rebound of the electrode due to stress release during cycling, reduces the probability of contact and short circuit between the negative and positive electrode films in the electrode, and reduces the amount of gas generated by electrolyte decomposition at high temperature. This reduces the probability of encapsulation failure near the current lead-out components, which is beneficial for improving the cycle performance of the pouch cell while maintaining high capacity. Battery devices with this pouch cell have good safety performance and high overall capacity.

[0018] In any embodiment, in the cross-section of the positive electrode film along the electrode thickness direction, the median L of the sphericity distribution curve of particles with a diameter greater than or equal to 1 μm is... A50 It is 0.67-0.75.

[0019] The median sphericity of particles with a diameter of 1 μm or greater within the above range is beneficial to reduce stress concentration caused by the irregularity of large particles, reduce the rebound of the electrode due to stress release during cycling, reduce the probability of contact and short circuit between the negative electrode film and the positive electrode film in the electrode, reduce the amount of gas generated by the electrolyte due to high temperature decomposition, thereby reducing the probability of encapsulation failure near the current lead-out component, which is beneficial to improve the capacity and cycle performance of the soft-pack battery cell, thereby improving the safety performance and overall capacity of the battery device.

[0020] In any embodiment, in the cross-section of the positive electrode film along the electrode thickness direction, the median L of the sphericity distribution curve of particles with a diameter greater than or equal to 1 μm is... A50 It is 0.69-0.75.

[0021] The median sphericity of particles with a diameter of 1 μm or greater is within the above range, which can further improve the stress concentration of large particles, reduce the rebound of the electrode due to stress release during cycling, further reduce the probability of contact and short circuit between the negative electrode film and the positive electrode film in the electrode, reduce the amount of gas generated by the electrolyte due to high temperature decomposition, thereby reducing the probability of encapsulation failure near the current lead-out component. The soft-pack battery cell has a high capacity, and the cycle performance of the soft-pack battery cell is further improved. The battery device has good safety performance and high overall capacity.

[0022] In any embodiment, the median C of the graphitization degree C in the cumulative distribution curve of the positive electrode film obtained in the laser microscopy confocal Raman spectroscopy instrument scanning mode is... 50 The value is 1.0-1.2, where the degree of graphitization C is I. G / I D , where I G This indicates that the Raman spectrum is at 1580±100 cm⁻¹ -1 The intensity of peak G at I D This indicates that the Raman spectrum is at 1350±100 cm⁻¹ -1 The intensity of peak D at that location.

[0023] In the cumulative distribution curve of graphitization degree C obtained by laser microscopy confocal Raman spectroscopy in instrument scanning mode, the median C of graphitization degree is... 50 Within the aforementioned range, the sliding rearrangement between particles can be promoted, thereby increasing the compaction density of the electrode sheet. This reduces the content of large particles in the positive electrode film, which helps to reduce the rebound phenomenon caused by excessive large particles in the film while maintaining the high capacity of the pouch cell. It further reduces the probability of contact and short circuit between the negative and positive electrode films in the electrode sheet, reduces the amount of gas generated by the electrolyte due to high-temperature decomposition, thereby reducing the probability of encapsulation failure near the current lead-out components, improving the cycle performance of the pouch cell, and giving the battery device good safety performance and high overall capacity.

[0024] In any embodiment, the median B of the coating value B obtained in the cumulative distribution curve of the positive electrode film layer in the laser microscopy confocal Raman spectroscopy instrument scanning mode is... 50 The value is 0.3-0.6, where the coating value B is I. P / I D , where I PThis indicates that the Raman spectrum is at 948±100 cm⁻¹ -1 The intensity of the P peak at I D This indicates that the Raman spectrum is at 1350±100 cm⁻¹ -1 The intensity of peak D at that location.

[0025] The median B of the coating value of the positive electrode film 50 Within the aforementioned range, the carbon material layer of the positive electrode active material is relatively dense and uniform, which is beneficial to improving the slip uniformity of the positive electrode film during the rolling process and reducing stress concentration in the positive electrode film. In addition, thanks to the dense and uniform carbon material layer, large particles in the positive electrode film are more likely to slip during the compaction process, thereby reducing stress concentration at large particles in the positive electrode film, reducing rebound caused by stress release at large particles during cycling, further reducing the probability of contact and short circuit between the negative electrode film and the positive electrode film in the electrode sheet, reducing the amount of gas generated by electrolyte decomposition at high temperature, thereby reducing the probability of encapsulation failure near the current lead-out component. On the basis of the high capacity of the soft-pack battery cell, the cycle performance of the soft-pack battery cell is further improved, and the battery device has good safety performance and high overall capacity.

[0026] In any embodiment, the lithium-containing transition metal phosphate particles include magnesium, and the mass content of magnesium is 1000ppm-3000ppm, optionally 1000ppm-2000ppm, based on the total mass of the lithium-containing transition metal phosphate particles in the positive electrode film.

[0027] Doping magnesium in positive electrode active materials can increase the Fe content in lithium iron phosphate materials. 3+ / Fe 2+ The concentration of coexisting states creates more electron-hole vacancies, thereby improving the electronic conductivity of the material. It also helps to broaden the lithium-ion diffusion channels, reduce Li+ migration resistance, and improve the rate performance of the soft-pack battery cells.

[0028] In any embodiment, the lithium-containing transition metal phosphate particles include titanium, and the mass content of titanium is 500ppm-8000ppm, optionally 1000ppm-3000ppm, based on the total mass of the lithium-containing transition metal phosphate particles in the positive electrode film.

[0029] In this embodiment, by adding a high content of titanium to lithium transition metal phosphate particles, the reactivity of the raw materials for synthesizing the positive electrode active material is reduced. This allows the positive electrode active material to achieve a high degree of graphitization while controlling the proportion of large particles, reducing stress concentration in the positive electrode film, and improving the rebound phenomenon caused by stress concentration at large particles. This further improves the cycle performance of the pouch battery cell while maintaining good capacity.

[0030] Meanwhile, the doping of titanium in the positive electrode active material is beneficial for inducing lattice distortion, reducing Li-O bond energy, increasing lithium-ion transport rate, and improving the kinetic performance of the battery. The uneven diffusion of lithium ions in the positive electrode film often involves a significant lithium-ion concentration gradient. This application's embodiments improve the solid-phase transport rate of the positive electrode active material by adding a high content of titanium to lithium-containing transition metal phosphate particles, thereby addressing the kinetic issues of the single-cell pouch battery.

[0031] In any embodiment, the lithium-containing transition metal phosphate particles include vanadium, and the mass content of vanadium is 500ppm-5000ppm, optionally 500ppm-3000ppm, based on the total mass of the lithium-containing transition metal phosphate particles in the positive electrode film.

[0032] Vanadium in the positive electrode film can be in multiple valence states, including +5 vanadium (V5). 5+ Vanadium (V+3) can be doped into phosphorus sites. Due to its large radius, it can cause lattice distortion, expand the diffusion channels of lithium ions, thereby improving the ionic conductivity of the positive electrode active material and enhancing the kinetic performance of the battery; 3+ Vanadium can be doped into transition metal sites, generating lithium vacancies through charge compensation, thereby improving the electronic conductivity of the positive electrode active material. Furthermore, the increased uniformity of vanadium distribution in lithium-containing transition metal phosphate particles helps to further improve the kinetic performance and reaction uniformity of the positive electrode film, thus further enhancing the kinetic and cycle performance of the pouch cell.

[0033] Vanadium content within the aforementioned range helps improve the kinetic performance of the positive electrode and the lithium transition metal phosphate battery. Simultaneously, the synergistic effect of titanium, vanadium, magnesium, and carbon nanotubes in the positive electrode film helps form a good three-dimensional network, further improving the electronic and ionic conductivity of the positive electrode film, thereby further enhancing the kinetic performance of the lithium transition metal phosphate pouch cell.

[0034] In any embodiment, when the pouch cell is fully discharged, the compaction density of the positive electrode sheet is 2.3 g / cm³. 3 -2.6g / cm 3 .

[0035] When a single pouch cell is fully discharged, the compaction density of the positive electrode sheet is less than 2.3 g / cm³. 3 When the battery is in a state of insufficient interparticle connection, it not only fails to achieve ideal capacity performance, but also hinders the formation of electron conduction networks and lithium-ion transport channels, significantly increasing the battery's internal resistance and leading to increased ohmic heat generation. Furthermore, when the compaction density of the positive electrode sheet of a single battery cell in a fully discharged state exceeds 2.6 g / cm³, the battery will not achieve the desired capacity performance.3 If the porosity of the positive electrode is too low, it will hinder lithium-ion diffusion and increase the electrochemical heat generation of the battery. Controlling the compaction density of the positive electrode within the above range is beneficial to improving the ohmic heat generation and electrochemical heat generation of the battery, thereby balancing the capacity and cycle performance of the pouch cell.

[0036] In any embodiment, the porosity of the positive electrode film is 14%-22%.

[0037] Porosity within the above-mentioned range of the positive electrode film layer is beneficial to improving the electrolyte retention characteristics, improving the ion diffusion of the large-particle positive electrode film layer with a certain area ratio, and improving the dynamic performance of the soft-pack battery cell.

[0038] In any embodiment, the positive electrode film layer further includes a conductive agent, the conductive agent including carbon nanotubes, the carbon nanotubes including one or more of single-walled carbon nanotubes, few-walled carbon nanotubes, and multi-walled carbon nanotubes, and the mass content of carbon nanotubes is 0.05%-2.5% based on the mass of the positive electrode film layer.

[0039] Carbon nanotubes have a high aspect ratio, which facilitates the bonding of multiple positive electrode particles in the thickness direction, forming a long-range conductive path while increasing the binding force between particles. This reduces local polarization and even lithium plating problems in pouch cell during cycling, thus improving the cycle life of pouch cell. Furthermore, through the binding effect, it reduces the rebound phenomenon of large particles in the positive electrode film, further reducing the probability of contact and short circuit between the negative electrode film and the positive electrode film in the electrode sheet. It also reduces the amount of gas generated by electrolyte decomposition at high temperature, thereby reducing the probability of encapsulation failure near the current lead-out components, further improving the cycle performance of pouch cell, and giving the battery device good safety performance.

[0040] Having a carbon nanotube content within the above range helps reduce the probability of excessive agglomeration of the conductive agent due to excessive carbon nanotube content, allowing it to be evenly distributed in the positive electrode film layer. This is beneficial for further improving the cycle performance of the pouch cell and enhancing the safety performance of the battery device.

[0041] In any embodiment, the conductive agent further includes conductive carbon black, the mass content of which is 0.05%-2.5% based on the mass of the positive electrode film.

[0042] Conductive carbon black, with its small size, adheres to the surface of positive electrode particles and fills the gaps between them, forming dense, dot-like conductive contacts. Its combination with carbon nanotubes balances long-range and short-range conductivity, further improving the conductive network within the positive electrode film. Simultaneously, the conductive agent's large specific surface area facilitates liquid absorption and retention, reducing electrolyte extrusion caused by high expansion forces during long cycles and improving the cycle life of individual pouch cells.

[0043] When the mass content of carbon nanotubes and conductive carbon black is within the above range, it can effectively alleviate the aggregation of carbon nanotubes and form a good conductive network structure, thereby effectively reducing the stress concentration of the positive electrode film and improving the liquid retention rate of the positive electrode film during long-term cycling. This further reduces the risk of electrode film detachment and polarization, improves the dynamic performance of the pouch cell, and enhances the cycle life of the pouch cell.

[0044] In any embodiment, based on the total area of ​​the cross-section of the positive electrode film along the thickness direction of the electrode sheet, the total area ratio of the agglomerated region of the conductive agent is 0.2%-6.0%, optionally 1.5%-5.0%; the agglomerated region of the conductive agent includes carbon nanotubes and conductive carbon black.

[0045] Based on the total area of ​​the cross-section of the positive electrode film along the thickness direction of the electrode sheet, the total area ratio of the agglomeration region of the conductive agent within the above range indicates that the conductive agent in the positive electrode film is uniformly dispersed and easy to form a uniform conductive network, which is beneficial to reduce the local polarization and even lithium plating problems generated by the soft-pack battery cells during cycling.

[0046] Meanwhile, research shows that large particles in lithium transition metal phosphates are prone to rebound. When the agglomeration area of ​​the conductive agent is within the above range, the uniform distribution of the conductive agent can suppress the rebound of lithium transition metal phosphate particles, form mechanical constraints on the particles and even the film layer, improve the cohesion of the film layer, reduce the damage of the SEI film and film layer during the rebound process, and improve the cycle life of the soft-pack battery cell.

[0047] In any embodiment, the thickness of the positive electrode film layer on one side is 70μm-120μm.

[0048] The specific capacity of lithium-containing transition metal phosphate particles is relatively low. Studies have shown that when the single-sided thickness of the positive electrode film is less than 70 μm, the capacity of the battery cell is difficult to meet market demand. A single-sided thickness of the positive electrode film within the aforementioned range is beneficial for improving the capacity of pouch cell batteries. However, increasing the thickness of the positive electrode film leads to longer electron and ion transport paths, increased resistance of the positive electrode film, and increased ohmic and electrochemical heat generation on the positive electrode. Controlling the thickness of the positive electrode film within a reasonable range is beneficial for improving the capacity of pouch cell batteries and further improving their cycle performance.

[0049] In any embodiment, the thickness of the positive electrode film layer on one side is 90μm-120μm.

[0050] The thickness of the positive electrode film on one side within the above range is beneficial to further improve the capacity of the individual soft-pack battery cells, thereby increasing the overall capacity of the battery device.

[0051] In any embodiment, the thickness of the positive electrode film layer on one side is 100μm-120μm.

[0052] Increasing the thickness of the positive electrode film on one side is beneficial to improving the capacity of the pouch cell. The applicant found that when the thickness of the positive electrode film on one side is greater than or equal to 100 μm, the phenomenon of particle rebound in the positive electrode film is more serious. The embodiments of this application effectively alleviate the serious rebound of the thick coating film during the cycle of the pouch cell. The pouch cell has good cycle performance while maintaining a high capacity.

[0053] In any embodiment, the length dimension L0 of the soft-pack battery cell is 500mm-1250mm; the width dimension W0 is 100mm-150mm; and the thickness dimension H0 is 14mm-22mm.

[0054] The dimensions of the soft-pack battery cells in this application embodiment are within the above-mentioned range, which is beneficial for achieving better capacity in the battery cells and improving the overall capacity of the battery device.

[0055] In any embodiment, the packaging bag includes an encapsulation layer, a metal layer, and a protective layer stacked sequentially from the inside of the battery cell to the outside of the battery cell, wherein the metal layer comprises aluminum; and the encapsulation layer and the protective layer comprise resin material.

[0056] Packaging bag materials containing the above-mentioned components have high elongation, which helps to improve the space utilization of battery cells, thereby increasing the energy density and capacity of battery cells. However, the composite material composed of aluminum and resin materials has poor thermal conductivity, resulting in low heat dissipation efficiency of pouch battery cells. Therefore, if the area ratio of large particles in the positive electrode film is too high, it will cause severe rebound phenomenon in the positive electrode film, leading to SEI film damage and film cracking. This can easily lead to misalignment between the positive and negative electrode plates and the separator, increasing the risk of local short circuits in the battery. Consequently, it will lead to increased local current density and temperature, accelerating electrolyte decomposition and increasing gas production, thus exacerbating the probability of encapsulation failure near the current lead. The embodiments of this application use the above-mentioned packaging bag and control the area ratio of large particles in the positive electrode film within a suitable range. The pouch battery cells have high capacity and good safety and cycle performance, and the battery device has high overall capacity and good safety performance.

[0057] In any embodiment, the encapsulation layer includes a polypropylene (PP) layer; optionally, the encapsulation layer includes a polypropylene (PP) layer and a modified polypropylene (PPa) layer disposed between the polypropylene (PP) layer and the metal layer; the protective layer includes one or more of nylon and polyethylene terephthalate (PET).

[0058] Modified polypropylene further improves the electrolyte corrosion resistance and bonding strength of the packaging bag. This encapsulation layer helps reduce interface leakage caused by insufficient heat sealing strength. The outer protective layer has excellent mechanical properties, which can buffer mechanical impact during assembly, reduce the risk of encapsulation failure of soft-pack battery cells, improve the safety performance of soft-pack battery cells, and thus improve the reliability of battery devices.

[0059] In any embodiment, the modified polypropylene (PPa) layer comprises maleic anhydride-grafted polypropylene.

[0060] Studies have shown that the main encapsulation failure sites near the current lead are the interfacial delamination between the polypropylene layer and the metal layer under high temperatures. The carboxyl groups (—COOH) and anhydride groups (—CO—O—CO—) of maleic anhydride can chemically bond with the hydroxyl groups (—OH) or alumina (Al2O3) on the aluminum foil surface, while simultaneously maintaining molecular chain entanglement with the polypropylene matrix. This helps to further improve the peel strength between the encapsulation layer and the metal layer, reducing the probability of delamination between the encapsulation layer and the metal layer under heat flow, lowering the risk of encapsulation failure in individual pouch cells, further improving the safety performance of pouch cell pouch cells, and enhancing the reliability of the battery device.

[0061] In any embodiment, the packaging bag is heat-sealed at 180°C-220°C.

[0062] The heat sealing temperature of the packaging bag is within the above range, which helps to enhance the interfacial bonding strength, reduce the probability of delamination between the encapsulation layer and the metal layer during battery cycling, reduce the risk of encapsulation failure of soft-pack battery cells, improve the safety performance of soft-pack battery cells, and improve the reliability of battery devices.

[0063] In any embodiment, the packaging bag is heat-sealed at 200°C-210°C.

[0064] The heat sealing temperature of the packaging bag is within the above range, which helps to further enhance the bonding strength between the encapsulation layer and the metal layer, thereby reducing the probability of delamination between the encapsulation layer and the metal layer during battery cycling, reducing the risk of encapsulation failure of soft-pack battery cells, improving the safety performance of soft-pack battery cells, and thus improving the reliability of battery devices.

[0065] In any embodiment, a thermal management component is provided between the support plate of the housing and the second surface of the soft-pack battery cell. The thermal management component is used to regulate the temperature of the soft-pack battery cell, and a thermally conductive structural adhesive is provided between the thermal management component and the second surface of the soft-pack battery cell.

[0066] The heat from a single pouch battery cell can be efficiently dissipated through thermal management components, which helps to further improve the cycle performance and safety performance of the pouch battery cell.

[0067] In any embodiment, at 85°C, the thermal conductivity of the thermally conductive structural adhesive is greater than or equal to 0.4 W / (m·K), and can be selected as 0.4 W / (m·K)-1.2 W / (m·K).

[0068] In any embodiment, the thermal conductivity of the thermally conductive structural adhesive is 0.8 W / (m·K)-1.2 W / (m·K) at 85°C.

[0069] The thermal conductivity of the thermally conductive structural adhesive is within the above range, which has good thermal conductivity and can still conduct heat stably at high temperatures. This helps reduce the probability of thermally conductive structural adhesive failure due to temperature rise, which in turn leads to the inability of heat to be transferred from the pouch cell to the thermal management component for heat dissipation in time, resulting in heat accumulation inside the cell. This is beneficial to improving the cycle performance of the pouch cell during long-term cycling.

[0070] In any embodiment, the thermally conductive structural adhesive has a storage modulus of 260MPa-1000MPa at a vibration frequency of 0.1Hz at room temperature, and can be optionally 300MPa-800MPa.

[0071] In any embodiment, the thermally conductive structural adhesive has a storage modulus of 300MPa-600MPa at a vibration frequency of 0.1Hz at room temperature.

[0072] At room temperature, the energy storage modulus at a vibration frequency of 0.1 Hz is within the above range. It has good mechanical properties and can reduce the probability of creep deformation or fatigue cracking of the thermally conductive structural adhesive under long-term mechanical vibration. This reduces the probability of displacement of the soft-pack battery cell and loss of its own thermal conductivity caused by the deformation of the thermally conductive structural adhesive. The thermally conductive structural adhesive can give full play to its good thermal conductivity and further improve the cycle performance of the soft-pack battery cell in the long cycle process.

[0073] In any embodiment, the glass transition temperature of the thermally conductive structural adhesive is 50°C-60°C.

[0074] When the glass transition temperature of the thermally conductive structural adhesive is within a suitable range, it is beneficial for the thermally conductive structural adhesive to fully exert its bonding and thermal conductivity, which is conducive to further improving the cycle performance of the soft-pack battery cells.

[0075] In any embodiment, the thermally conductive structural adhesive comprises a polyurethane resin and thermally conductive filler particles dispersed in the polyurethane resin; the thermally conductive filler particles comprise one or more of aluminum hydroxide particles and boron nitride particles.

[0076] Thermally conductive structural adhesives containing the above components exhibit good high-temperature resistance.

[0077] In any embodiment, based on the total mass of the thermally conductive structural adhesive, the mass percentage of the thermally conductive filler particles is 20%-70%, optionally 45%-65%.

[0078] The thermally conductive filler particles in the thermally conductive structural adhesive are within the above-mentioned range, which is beneficial to improving the thermal conductivity of the thermally conductive structural adhesive and reducing the problem of insufficient resin content caused by excessive thermally conductive filler particles, which would result in poor energy storage modulus of the thermally conductive structural adhesive. The thermally conductive structural adhesive has good thermal conductivity, which is beneficial to improving the cycle performance of soft-pack battery cells.

[0079] In any embodiment, the projection of the thermally conductive structural adhesive on the first surface does not overlap with the projection of the negative electrode sheet on the first surface.

[0080] After the battery cells are bonded to the thermally conductive structural adhesive, the adhesive may overflow. Once the battery cells are assembled into a battery device, the projection of the thermally conductive structural adhesive on the first surface does not overlap with the projection of the negative electrode sheet on the first surface. This reduces the probability of the relatively rigid thermally conductive structural adhesive and the electrode sheet directly compressing each other during battery cycling, lowering the probability of stress concentration on the battery electrode sheet caused by the thermally conductive structural adhesive, thereby reducing the adverse impact on the cycle performance of the pouch battery cells.

[0081] In any embodiment, at least some of the pouch cell units are provided with double-sided adhesive, and a gap is provided between the double-sided adhesive and the thermally conductive structural adhesive.

[0082] After the battery cells are bonded to the thermally conductive structural adhesive, excess adhesive may appear. The battery cells are then bonded together using double-sided adhesive. After assembling them into a battery device, a gap is created between the double-sided adhesive and the thermally conductive structural adhesive. This reduces the probability of the relatively rigid thermally conductive structural adhesive and the double-sided adhesive coming into contact with each other during battery cycling. This reduces stress concentration caused by the rigid thermally conductive structural adhesive on the double-sided adhesive between the battery cells, thereby minimizing any adverse impact on the cycle performance of the pouch battery cells.

[0083] A second aspect of this application provides an electrical device, including the battery device provided in the first aspect of this application, the battery device being used to provide electrical energy.

[0084] A third aspect of this application provides an energy storage device, including the battery device provided in the first aspect of this application, wherein the battery device is used to store electrical energy. Attached Figure Description

[0085] Figure 1 is a schematic diagram of a battery device according to an embodiment of this application;

[0086] Figure 2 is a partial enlarged view of a battery device according to an embodiment of this application;

[0087] Figure 3 is an enlarged view of the battery device shown in Figure 2 at box B;

[0088] Figure 4 is a partial enlarged view of a battery device according to another embodiment of this application;

[0089] Figure 5 is a schematic diagram of a battery cell according to an embodiment of this application;

[0090] Figure 6 is a cross-sectional view of the battery cell shown in Figure 5;

[0091] Figure 7 is an enlarged view of the battery cell shown in Figure 6 at box A;

[0092] Figure 8 is a schematic diagram of a packaging bag according to an embodiment of this application;

[0093] Figure 9 is a schematic diagram of an electrical device according to an embodiment of this application.

[0094] Explanation of reference numerals in the attached drawings: 10 Battery assembly; 1 Housing; 11 Support plate; 12 Connecting beam; 2 Soft-pack battery cell; 21 First surface; 22 Second surface; 201 Packaging bag; 202 Electrode assembly; 203 Current lead; 204 Tab; 221 Protective layer; 222 Metal layer; 223 Encapsulation layer; 3 Thermal management component; 4 Thermally conductive structural adhesive; X First direction; Y Second direction; Z Third direction. Detailed Implementation

[0095] The following detailed description, with appropriate reference to the accompanying drawings, specifically discloses embodiments of the battery device, power-consuming device, and energy storage device of this application. However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repetitive descriptions of practically identical structures may be omitted. This is to avoid unnecessarily lengthy descriptions and to facilitate understanding by those skilled in the art. Furthermore, the accompanying drawings and the following description are provided for the purpose of enabling those skilled in the art to fully understand this application and are not intended to limit the subject matter of the claims.

[0096] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values ​​of 1 and 2 are listed, and if maximum range values ​​of 3, 4, and 5 are listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0097] Unless otherwise specified, all embodiments and optional embodiments of this application may be combined with each other to form new technical solutions, and such technical solutions should be considered to be included in the disclosure of this application.

[0098] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions, and such technical solutions shall be deemed to be included in the disclosure of this application.

[0099] Unless otherwise specified, all steps in this application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the method may also include step (c), indicating that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.

[0100] In this application, the terms "multiple" or "various" refer to two or more kinds of things.

[0101] Unless otherwise stated, the terms used in this application have the common meanings as commonly understood by those skilled in the art.

[0102] Unless otherwise stated, the values ​​of the parameters mentioned in this application can be determined using various testing methods commonly used in the art, for example, according to the testing methods given in the embodiments of this application. Unless otherwise stated, the test temperature for each parameter is 25°C.

[0103] In embodiments of this application, the battery device includes multiple battery cell assemblies for providing voltage and capacity. A battery cell assembly may include multiple pouch cell batteries, which are connected in series, parallel, or mixed connections via a busbar. For example, a battery cell assembly is typically formed by arranging multiple pouch cell batteries; a battery cell assembly may also be a battery module, which is formed by arranging and fixing multiple pouch cell batteries into an independent module.

[0104] The battery device can be a battery pack, which includes a housing and multiple individual battery cells housed within the housing. The individual battery cells can be battery modules, which are housed within the housing by directly fixing multiple pouch cells to it.

[0105] In embodiments of this application, the housing can be part of the vehicle's chassis structure. For example, a portion of the housing can be at least a part of the vehicle's floor, or a portion of the housing can be at least a part of the vehicle's crossbeams and longitudinal beams.

[0106] In this embodiment, the battery cell can be a rechargeable battery, which refers to a battery cell that can be recharged after discharge to activate the active materials and continue to be used; the battery cell can be a lithium-ion battery. The battery cell can be flat.

[0107] In some implementations, the battery can be an energy storage device. Energy storage devices include energy storage containers, energy storage cabinets, etc.

[0108] In some embodiments, individual battery cells can be assembled into battery modules, and the number of battery cells contained in a battery module can be multiple, with the specific number adjustable according to the application and capacity of the battery module. In some embodiments, the above-mentioned battery modules can also be assembled into battery packs, and the number of battery modules contained in the battery packs can be adjusted according to the application and capacity of the battery packs.

[0109] A single battery cell includes electrode components and an electrolyte.

[0110] Electrode assemblies typically include positive and negative electrodes. The negative electrode is the electrode that absorbs or lithiates lithium ions during charging and releases or delithiates lithium during discharging. The positive electrode is the electrode that absorbs or delithiates lithium ions during charging and absorbs or lithiates lithium during discharging.

[0111] To meet the market demand for high-capacity battery devices, pouch cell batteries have advantages such as light weight, flexible design, and high energy density. Furthermore, the applicant discovered that by directly integrating multiple pouch cell batteries in a module-free manner, the traditional module structure is eliminated, and the reduction of redundant components helps to improve space utilization, thereby further increasing the battery capacity.

[0112] Soft-pack batteries are sealed in packaging bags and contain electrode assemblies. These assemblies require current leads to connect to the external circuitry. The packaging bag is sealed to the current leads. The current leads conduct current, but the connection area between the current leads and the tabs in the electrode assembly is often limited, resulting in high current density and heat generation in the overcurrent region. The module-less design makes it even more difficult for heat to dissipate or be conducted quickly. Heat is rapidly transferred to the packaging bag at the connection point with the current leads. During high-rate charging and discharging or under long-term charging and discharging, the packaging bag and / or encapsulating adhesive near the current leads are prone to polymer creep, leading to encapsulation failure in the vicinity of the current leads.

[0113] Such encapsulation failure can compromise the airtightness of individual battery cells, leading to battery performance degradation; it can even cause gases and liquid electrolytes generated by the thermal decomposition of the internal electrolyte to escape from the failure site, posing a safety risk. Simultaneously, the module-less integration method makes the arrangement of pouch cell batteries more compact, further limiting heat dissipation space and making heat more prone to accumulation, increasing the risk of heat seal failure and thermal runaway. How to obtain battery devices that simultaneously possess good capacity and safety performance is a pressing technical problem that needs to be solved in this field.

[0114] The first aspect of this application provides a battery device 10, as shown in Figures 1 to 7. The battery device 10 includes a housing 1; the housing 1 includes a support plate 11 and a frame surrounding the outer periphery of the support plate 11, the support plate 11 being fixedly connected to the frame; a plurality of pouch battery cells 2, the plurality of pouch battery cells 2 being stacked in a first direction X and housed within the housing 1; the rated capacity of each pouch battery cell 2 is greater than or equal to 50 Ah and less than or equal to 300 Ah; the surface of each pouch battery cell 2 includes a first surface 21 and a second surface 22, the area of ​​the first surface 21 being greater than the area of ​​the first surface 21. The area of ​​the second surface 22 is described above. The first surfaces 21 of the plurality of soft-pack battery cells 2 are arranged opposite each other along the first direction X. The support plate 11 and the second surfaces 22 of the plurality of soft-pack battery cells 2 are arranged opposite each other along the second direction Y. At least one connecting beam 12 extending along the third direction Z is provided inside the housing 1. The connecting beam 12 is fixedly connected to the support plate 11 and / or the frame. At least one soft-pack battery cell 2 abuts against the connecting beam 12 along the first direction X. The first direction X, the second direction Y, and the third direction Z are perpendicular to each other. In this embodiment, the soft-pack battery cell 2 includes a packaging bag 201, an electrode assembly 202, and a current lead 203. The electrode assembly 202 is housed within the packaging bag 201. One end of the current lead 203 is connected to the electrode assembly 202, and the other end of the current lead 203 is located outside the packaging bag 201. The current lead 203 and the packaging bag 201 are encapsulated and connected. The electrode assembly 202 includes a positive electrode, a negative electrode, and a separator disposed between the positive and negative electrode. The positive electrode includes a positive current collector and a separator disposed between the positive and negative electrode. The positive electrode current collector has a positive electrode film layer on at least one side, the positive electrode film layer comprising a positive electrode active material, the positive electrode active material comprising lithium transition metal phosphate particles with carbon material disposed on at least a portion of its surface; in the cross-section of the positive electrode film layer along the thickness direction of the electrode sheet, the area ratio of particles with a particle size greater than or equal to 1 μm is 12%-40%; the separator comprises a base film and ceramic layers disposed on both sides of the base film and an adhesive layer disposed on the side of the ceramic layer away from the base film, at least on the side close to the positive electrode sheet, the adhesive layer being a continuous layer with a porous structure, the adhesive layer comprising a vinylidene fluoride polymer. In this application, at least one of the pouch cell abuts against the connecting beam along the first direction means that the pouch cell and the connecting beam can be in direct or indirect contact, but the direction of the force between them is basically along the first direction.

[0115] The enclosure is supported by a support plate and a frame set on the outer periphery of the support plate, which helps to reduce the weight of the enclosure in the battery device and achieve lightweighting. However, it also weakens the stability of the battery device. At least one connecting beam extending along a third direction is provided in the enclosure. The connecting beam abuts against the battery cell along the first direction and provides support force to the battery cell. This can improve the rigidity of the battery device and improve the structural stability of the battery device while maintaining its lightweight.

[0116] It is understood that the fact that the support plate and the second surface of the plurality of pouch battery cells are arranged opposite each other along the second direction means that the surface of the support plate and the second surface of the battery cells are opposite each other along the second direction, and does not necessarily mean that the two are in contact with each other.

[0117] In some embodiments, a thermal management component is provided between the support plate and the second surface of the plurality of pouch cell cells.

[0118] In some embodiments, the support plate is bonded to the second surface of the plurality of pouch cell cells.

[0119] Soft-pack batteries have low mechanical strength and poor resistance to internal pressure. Furthermore, after the soft-pack battery cells are integrated with the casing in a module-free design, there are no modules separating a large number of battery cells. The pollution caused by the failure of the encapsulation of a single battery cell is far greater than that of a traditional module. Therefore, lithium transition metal phosphate systems, which have high safety and relatively low gas production, are particularly suitable for soft-pack batteries.

[0120] However, lithium-containing transition metal phosphates are limited by specific capacity, requiring increased compaction to improve capacity and overcome the energy density bottleneck. Furthermore, when the rated capacity of a single pouch cell is less than 50 Ah, it is difficult to meet the power requirements of the battery device. When the rated capacity of a single pouch cell is greater than 300 Ah, higher capacity often requires thicker electrodes or larger electrode areas, and Joule heat and reaction heat increase significantly with increasing capacity, severely deteriorating the safety performance of the pouch cell. The applicant has discovered that a certain proportion of particle size distribution is beneficial to improving the compaction density of the positive electrode film, achieving a rated capacity of greater than or equal to 50 Ah and less than or equal to 300 Ah for each pouch cell, ensuring a considerable overall capacity of the battery device. Specifically, when the area ratio of particles with a diameter greater than or equal to 1 μm in the cross-section of the positive electrode film along the electrode thickness direction is less than 12%, insufficient particle size distribution will significantly limit the potential for increasing compaction density, thus failing to meet the design requirements for the capacity of the pouch cell. The applicant also discovered that when the area of ​​particles with a diameter greater than or equal to 1 μm in the cross-section of the positive electrode film along the thickness direction of the electrode sheet is greater than 50%, the excessive large particles will cause a severe rebound phenomenon in the positive electrode film, leading to SEI film damage and film layer cracking. This can easily cause misalignment between the positive and negative electrode sheets and the separator, increasing the risk of local short circuit in the battery. Consequently, it can lead to an increase in local current density and temperature, accelerate electrolyte decomposition, and increase gas production, thereby exacerbating the probability of encapsulation failure near the current lead-out components.

[0121] This application improves the battery capacity by using lithium transition metal phosphate (LiMT) pouch cell integrated with a module-free approach. It further utilizes a separator with ceramic layers on both sides to increase separator stiffness. Simultaneously, it employs a continuous porous separator with a larger bonding area and stronger adhesion to enhance the bonding between the separator and the positive electrode, improving the density and stiffness of the internal electrode assembly. This compensates for the weak external binding force of the electrode assembly and reduces the risk of horizontal misalignment due to mutual compression of the positive and negative electrode sheets in the thickness direction during rebound. Furthermore, by controlling the area ratio of large-diameter LiMT particles in the positive electrode film to within 12%-40%, it improves the particle size distribution of the film and reduces rebound phenomena caused by excessive large particles, lowering the risk of positive and negative electrode overlap and subsequent short circuits. It also reduces the amount of gas generated by electrolyte decomposition at high temperatures, thereby reducing the probability of encapsulation failure near the current leads and improving the safety performance of the pouch cell. The embodiments of this application improve the overall capacity and safety performance of the battery device through a module-free integration method and the synergistic design of the soft-pack battery cell, positive electrode plate and separator.

[0122] In some implementations, end plates or side plates are provided on the frame.

[0123] In some implementations, neither end plates nor side plates are provided on the frame.

[0124] In some embodiments, as shown in FIG7, the electrode assembly 202 includes a tab 204, one end of a current lead 203 is connected to the tab 204, and the other end of the current lead 203 is located outside the packaging bag 201.

[0125] In this application, the rated capacity of a single pouch battery cell has a meaning known in the art, and can be tested using methods known in the art or obtained from the battery device instruction manual. As an example, at 25°C, the battery cell is charged to 3.65V at a charging rate of 0.5C (the nominal capacity of the cell), then charged at a constant voltage of 3.65V to 0.05C, left to stand for 10 minutes, and then discharged to 2.5V at a discharging rate of 1C, left to stand for 10 minutes. The capacity C during the discharge process is calculated using the formula C = I × t, with the unit being Ah.

[0126] Lithium-containing transition metal phosphate particles refer to phosphate materials containing lithium and transition metal elements, and can be detected by any method known in the art. For example, they can be detected by combining X-ray diffraction (XRD) with energy dispersive spectroscopy (EDS) or inductively coupled plasma mass spectrometry (ICP-MS).

[0127] It should be noted that the positive electrode film layer contains lithium transition metal phosphate particles, but the positive electrode film layer does not only refer to the positive electrode active material layer. Other film layers that are connected to the positive electrode active material layer and are difficult to distinguish, such as the undercoat layer and the liquid retention layer, are all collectively referred to as the positive electrode film layer.

[0128] In this application, the term "particle" refers to a particle in the positive electrode film layer that has a recognizable complete boundary in the field of view at a certain magnification, such as 10,000x. Defects and scratches may exist inside the particle, but a complete boundary sufficient to divide the particle cannot be identified inside the particle.

[0129] The particle identification method is as follows: The positive electrode film layer is cut along the thickness direction of the electrode sheet using an argon ion beam (for example, a Leica EM TIC 3X CP device can be used, operating voltage: 6kV, operating time: 6h). After exposing the cut surface, a scanning electron microscope (SEM) is used (for example, a Hitachi SU8230 device can be used, operating voltage: 3kV, beam current: high, probe model: U (LA100), working distance <5mm) to observe the cut surface along the thickness direction of the electrode sheet. Images are acquired using a field emission scanning electron microscope at a non-edge location in the cut surface of the positive electrode film layer (after observing the electrode edge under the SEM, the field of view is adjusted to the center of the sample) in secondary electron mode. Electron micrographs are taken at 10kx magnification, and the particles in the electron micrographs are analyzed using ImageJ software (1.46r, win64 version). The specific steps for using ImageJ software are as follows: Load the scanning electron microscope (SEM) image to be analyzed; use the Cellpose plugin to identify particles, and then perform manual corrections; use ImageJ to read and analyze data. The specific method for using the Cellpose plugin to identify particles is as follows: Set the segmentation diameter parameter (diameter in the Segmentation module) to 15 pixels, click "run cyto3" to identify particles; manually mark particles in the image that were not identified by the software, were not fully identified, or were identified incorrectly. Particles that were not identified by the software, were not fully identified, or were identified incorrectly mainly include the following: 1. Particles that are too large or have scratches on their surface, making them unidentifiable or incompletely identifiable; 2. During argon ion beam cutting, scratches may be generated on the particle surface, and the software may misinterpret these scratches as particle boundaries, leading to identification errors; 3. Particles that are too small and were not successfully identified; 4. Particles located at the edge of the SEM field of view, with the particle's interior penetrated by the edge, preventing a complete view of the morphology, resulting in identification errors due to partial identification replacing the whole.For the unidentified or misidentified particles mentioned above, manual calibration is performed. The specific process is as follows: 1. Delete large particles located around the edges of the scanning electron microscope that are not fully displayed. 2. Determine if any unidentified or misidentified particles have internal cracks or scratches. If no cracks or scratches are found, classify it as a single particle and manually mark it based on the observed particle boundary. 3. If cracks or scratches are found inside the particle, determine if they penetrate the particle. If not, classify it as a single particle and manually mark it. 4. If cracks or scratches penetrate the particle, determine if they are linear or irregular. 5. If the cracks or scratches are irregular, classify them as the boundary between particles and divide the particles along this boundary. 6. If the cracks or scratches are linear, perform contrast comparison. 7. If the contrast is not obvious and there is no crack-like appearance, classify it as a scratch and mark it as a single particle. 8. If the contrast is strong and there is a crack-like appearance, classify it as the boundary between particles and mark it as two particles. After manual marking, delete information irrelevant to the particles from the automatic image processing, thus completing the particle identification and marking in the image.

[0130] It is understandable that particles larger than 50 nm, especially in the cross-section of the positive electrode film along the electrode thickness direction, mainly originate from the positive electrode active material. Therefore, the embodiments of this application can accurately and objectively reflect the distribution of lithium transition metal phosphate particles within the positive electrode film by observing and statistically analyzing the particle area in the cross-section of the positive electrode film along the electrode thickness direction.

[0131] In existing technologies, laser particle size analyzers are typically used to statistically analyze the particle size of positive electrode active materials using Malvern laser diffraction. However, the applicant's research indicates that because lithium-containing transition metal phosphate particles are prone to agglomeration, the test results obtained by Malvern laser diffraction based on the principle of laser scattering often only reflect the particle size of the agglomerates, and cannot accurately reflect the particle size of the positive electrode active material, let alone its dispersion state in the film layer. This is because the dispersion of the positive electrode active material in the film layer increases during slurry preparation and film forming rolling. The test results obtained by Malvern laser diffraction are affected by the particle size, specific surface area, and degree of agglomeration of the positive electrode active material. Compared to the actual dispersion in the electrode sheet, the number of large particles obtained by this test is lower than the actual value, and the number of small particles is higher than the actual value. Therefore, the particle size obtained by Malvern laser diffraction cannot be equated with or analogized to the particle size statistically obtained in the embodiments of this application.

[0132] The specific method for testing the area ratio of particles with a diameter greater than or equal to 1 μm in the cross-section of the positive electrode film along the electrode thickness direction is as follows: Particles in the cross-section of the positive electrode film along the electrode thickness direction are identified according to the method described above in this application. The images after particle identification and labeling are imported into ImageJ software for analysis. The scale is set based on the scanning electron microscope image. The particle size, area, sphericity, and roughness of the particles in the cross-section along the electrode thickness direction are statistically analyzed using the "Feret," "Area," "Round," and "Solidity" analysis functions. According to the software manual (ImageJ User Guide IJ 1.46r), the obtained "Feret" parameter represents the maximum spacing between all parallel lines in the two-dimensional projection of the particle, thus characterizing the particle size; the obtained "Area" parameter represents the pixel area of ​​the particle. Because particles smaller than 50 nm are prone to significant errors during statistical analysis and are difficult to accurately identify, and because the particle size of conductive agents is generally smaller than 50 nm, which can also introduce large errors into the statistical results, particles smaller than 50 nm are not counted in the particle size statistics of this application, and the particle statistics corresponding to Area, Round, or Solidity values ​​displaying as "NaN" are deleted. The sum of the "Area" parameters of particles with a diameter greater than or equal to 1 μm and the sum of the "Area" parameters of all particles are calculated and used as the area of ​​particles with a diameter greater than or equal to 1 μm and the total area of ​​the counted particles, respectively. The sum of the areas of particles with a diameter greater than or equal to 1 μm divided by the total area of ​​the counted particles is used as the percentage of the area of ​​particles with a diameter greater than or equal to 1 μm in the cross-section of the positive electrode film along the thickness direction of the electrode sheet.

[0133] In some embodiments, the area percentage of particles with a diameter greater than or equal to 1 μm in the cross-section of the positive electrode film along the electrode thickness direction can be selected as 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39%, 40%, or any value range between the two.

[0134] In some embodiments, the rated capacity of each of the pouch cell can be selected as 50Ah, 60Ah, 70Ah, 80Ah, 90Ah, 100Ah, 110Ah, 120Ah, 130Ah, 140Ah, 150Ah, 160Ah, 170Ah, 180Ah, 190Ah, 200Ah, 210Ah, 220Ah, 230Ah, 240Ah, 250Ah, 260Ah, 270Ah, 280Ah, 290Ah, 300Ah, or any value range between the two.

[0135] In some embodiments, the vinylidene fluoride polymer includes one or more of vinylidene fluoride homopolymer (PVDF) and copolymers of vinylidene fluoride and hexafluoropropylene.

[0136] In the prior art, the adhesive layer of the diaphragm often uses aqueous PVDF, which often presents an island-like structure in the diaphragm. This is beneficial for providing gaps for cell expansion and is also convenient for manufacturing. However, such diaphragm adhesive layers have low bonding area and weak adhesion.

[0137] The adhesive layer of the separator in this embodiment has a certain porous structure in its continuous structure, through which the ceramic layer disposed between the base film and the adhesive layer can be observed. It is understood that when a porous continuous layer is used as the adhesive layer, it may become blocky due to contact with the positive or negative electrode or under pressure during electrode manufacturing or cycling. The continuous layer referred to in this application does not require the adhesive layer to be continuous throughout the entire battery; rather, it refers to a continuous layer with a uniform porous structure at the microscopic level, such as when observed under a microscope, rather than an island-like structure. To reflect the true morphology of the separator, during sampling, it is preferable to sample in areas of the battery where the separator adhesive layer has minimal adhesion to the positive or negative electrode. For example, sampling can be performed at the location of the separator where the projection extends beyond the positive and negative electrode; or sampling can be performed on the separator near the surface of the electrode assembly. The separator sampled in this way better reflects the true state of the separator.

[0138] The separator provided in this application uses a continuous porous layer as the adhesive layer, which has a larger bonding area compared to the island-shaped adhesive layer in the prior art. This results in a stronger and more uniform bond between the separator and the positive electrode film. Simultaneously, the porous structure in the adhesive layer allows for both lithium-ion transport efficiency and improved battery dynamics. Lithium-containing transition metal phosphate particles with a particle size greater than or equal to 1 μm can damage the SEI film and electrode film during rebound. Furthermore, the mutual compression of the positive and negative electrode films in the thickness direction can easily cause relative misalignment in the horizontal direction, increasing the risk of local short circuits in the battery. This leads to increased local current density, higher temperature, and accelerated electrolyte decomposition, resulting in increased gas production. The separator provided in this application has ceramic layers on both sides and uses a continuous porous layer as the adhesive layer. This helps reduce the rebound phenomenon of the electrode assembly during long-cycle operation, reduces the risk of positive and negative electrode overlap leading to short circuits, reduces the amount of gas produced by electrolyte decomposition at high temperatures, and thus reduces the probability of encapsulation failure near the current lead, improving the safety performance of the pouch battery cell.

[0139] This application embodiment uses a continuous layer with a porous structure as an adhesive layer to improve the adhesion between the separator and the electrode while maintaining the air permeability and porosity of the separator, improve the stability of the electrode, further reduce the risk of internal short circuit caused by electrode rebound, reduce the amount of gas generated by electrolyte decomposition at high temperature, thereby reducing the probability of encapsulation failure near the current lead-out component and improving the safety performance of the soft-pack battery cell.

[0140] In some embodiments, the base film may be made of one or more of the following materials, including but not limited to glass fiber, nonwoven fabric, polyethylene (PE), and polypropylene (PP).

[0141] In this application, the ceramic layer includes ceramic particles, which include one or more of Al2O3, AlO(OH), SiO2, TiO2, MgO, CaO, ZnO2, ZrO2, and SnO2.

[0142] Ceramic particles possess flame retardancy and high hardness, making them resistant to deformation under heat and exhibiting excellent dimensional stability. Placing ceramic layers on both sides of the base film enhances battery rigidity, reduces electrode rebound, and decreases the probability of short circuits caused by contact between the negative and positive electrode films during rebound. This, in turn, reduces gas generation from electrolyte decomposition at high temperatures, thereby decreasing the probability of encapsulation failure near current leads and improving the safety performance of individual pouch cells.

[0143] In some embodiments, the rated capacity of each of the pouch cell is greater than or equal to 100 Ah and less than or equal to 200 Ah.

[0144] The rated capacity of each of the aforementioned pouch cell is within the above-mentioned range, which is beneficial to improving the overall capacity of the battery device.

[0145] In some embodiments, the area ratio of particles with a diameter of 1μm-5μm in the cross-section of the positive electrode film along the thickness direction of the electrode sheet is 12%-37%.

[0146] When the area ratio of particles with a diameter of 1μm-5μm in the cross-section of the positive electrode film along the thickness direction of the electrode sheet is within the above range, it is beneficial for the soft-pack battery cell to maintain high capacity while further improving the electrode rebound phenomenon caused by stress concentration of large particles in the electrode sheet. This reduces the probability of contact and short circuit between the negative electrode film layer and the positive electrode film layer in the electrode sheet, reduces the amount of gas generated by electrolyte decomposition at high temperature, thereby reducing the probability of encapsulation failure near the current lead-out component, improving the cycle performance of the soft-pack battery cell, and the battery device with this soft-pack battery cell has good safety performance and high overall capacity.

[0147] In some embodiments, in the cross-section of the positive electrode film along the electrode thickness direction, the median L of the spheroidality in the cumulative distribution curve of the spheroidality area of ​​particles with a diameter greater than or equal to 1 μm is... A50 It is 0.6-0.8.

[0148] The specific method for testing the sphericity of particles with a diameter greater than or equal to 1 μm in a cross-section of the positive electrode film along the electrode thickness direction is as follows: Particles with a diameter greater than or equal to 1 μm in a cross-section of the positive electrode film along the electrode thickness direction are identified using the method described above in this application. The morphology of the particles in the cross-section along the electrode thickness direction of the positive electrode film is analyzed using the "Shape Description" analysis function in ImageJ. According to the software manual (ImageJ User Guide IJ 1.46r), the "Round" parameter obtained from the analysis represents the ratio of the pixel area of ​​the particle to the area of ​​a circle with the fitted major axis as its diameter, which can be used to characterize the sphericity of the particle. The closer the particle is to a sphere, the closer the ratio of the pixel area to the area of ​​the circle with the fitted major axis as its diameter is to 1. Therefore, the "Round" parameter of the particle obtained from the analysis is used to characterize the sphericity of the particle. Because particles smaller than 50 nm present significant errors during statistical analysis and are difficult to accurately identify, and because the particle size of conductive agents is generally smaller than 50 nm, which can also introduce substantial errors into the statistical results, particles smaller than 50 nm are not counted in the particle size statistics process of this application, and the statistical data for particles with a Round value of "NaN" are deleted. Following the above method, to ensure a statistically significant sample size, at least 10 non-overlapping scanning electron microscope (SEM) images were acquired for each electrode. The sphericity of at least 1000 particles was arranged in ascending order, and the cumulative sphericity distribution curve of the particles in the positive electrode film was obtained with sphericity as the horizontal axis and the cumulative area percentage as the vertical axis. A50 This is the L-value of sphericity that corresponds to the cumulative area ratio of the vertical axis in the cumulative distribution curve of granular sphericity L-values ​​being 50%.

[0149] In some embodiments, in the cross-section of the positive electrode film along the electrode thickness direction, the median L of the spheroidality in the cumulative distribution curve of the spheroidality area of ​​particles with a diameter greater than or equal to 1 μm is... A50 The value can be selected from 0.60, 0.61, 0.62, 0.63, 0.64, 0.65, 0.66, 0.67, 0.68, 0.69, 0.70, 0.705, 0.71, 0.72, 0.73, 0.74, 0.75, 0.76, 0.77, 0.78, 0.79, 0.80, or any value range between the two.

[0150] The median sphericity of particles with a diameter of 1 μm or greater is within the above range. Larger particles have better sphericity, reducing particle bridging caused by irregular particle shape, and reducing stress concentration exacerbated by the irregularity of large particles. This reduces the rebound of the electrode due to stress release during cycling, reduces the probability of contact and short circuit between the negative and positive electrode films in the electrode, and reduces the amount of gas generated by electrolyte decomposition at high temperature. This reduces the probability of encapsulation failure near the current lead-out components, which is beneficial for improving the cycle performance of the pouch cell while maintaining high capacity. Battery devices with this pouch cell have good safety performance and high overall capacity.

[0151] Those skilled in the art can control the sphericity of particles using any known process. For example, the sphericity of particles can be adjusted through processes such as grinding, polishing, chemical etching, mechanical stirring, extrusion, coating, granulation, and adding surfactants, as well as by adjusting the parameters of each process.

[0152] In some embodiments, in the cross-section of the positive electrode film along the electrode thickness direction, the median L of the spheroidality in the cumulative distribution curve of the spheroidality area of ​​particles with a diameter greater than or equal to 1 μm is... A50 It is 0.67-0.75.

[0153] The median sphericity of particles with a diameter of 1 μm or greater within the above range is beneficial to reduce stress concentration caused by the irregularity of large particles, reduce the rebound of the electrode due to stress release during cycling, reduce the probability of contact and short circuit between the negative electrode film and the positive electrode film in the electrode, reduce the amount of gas generated by the electrolyte due to high temperature decomposition, thereby reducing the probability of encapsulation failure near the current lead-out component, which is beneficial to improve the capacity and cycle performance of the soft-pack battery cell, thereby improving the safety performance and overall capacity of the battery device.

[0154] In some embodiments, in the cross-section of the positive electrode film along the electrode thickness direction, the median L of the spheroidality in the cumulative distribution curve of the spheroidality area of ​​particles with a diameter greater than or equal to 1 μm is... A50 It is 0.69-0.75.

[0155] The median sphericity of particles with a diameter of 1 μm or greater is within the above range, which can further improve the stress concentration of large particles, reduce the rebound of the electrode due to stress release during cycling, further reduce the probability of contact and short circuit between the negative electrode film and the positive electrode film in the electrode, reduce the amount of gas generated by the electrolyte due to high temperature decomposition, thereby reducing the probability of encapsulation failure near the current lead-out component. The soft-pack battery cell has a high capacity, and the cycle performance of the soft-pack battery cell is further improved. The battery device has good safety performance and high overall capacity.

[0156] In some embodiments, the median C of the graphitization degree C in the cumulative distribution curve of the positive electrode film obtained in laser microscopy confocal Raman spectroscopy instrument scanning mode is... 50 The value is 1.0-1.2; where the degree of graphitization C is I. G / I D I G This indicates that the Raman spectrum is at 1580±100 cm⁻¹ -1 The intensity of peak G at I D This indicates that the Raman spectrum is at 1350±100 cm⁻¹ -1 The intensity of peak D at that location.

[0157] In this application, the graphitization degree C value of the positive electrode film can be obtained by surface scanning mode of a laser confocal Raman spectrometer. As an example, specifically, a laser confocal Raman spectrometer (high-precision Renishaw laser confocal Raman spectrometer) is used, with an excitation wavelength of 532 nm. An appropriate amount of the positive electrode film is taken and surface scanned on its surface or along the cross-section of the electrode thickness. The scanning area is 45 μm × 45 μm, divided into 10 × 10 grids, with grid vertices as test points, a step size of 5 μm, and a total of 100 scan points. Thus, the C values ​​at different sites and the cumulative distribution curve of the C values ​​in the surface scan area are obtained.

[0158] The positive electrode film in this application can be either a freshly prepared positive electrode film or a positive electrode film obtained from disassembly of a battery. The surface of a positive electrode film obtained from disassembly of a battery inevitably contains residual electrolyte salt particles. To improve testing accuracy, it is preferable to perform a surface scan on a cross-section of the positive electrode film along the electrode thickness direction to characterize the degree of graphitization of the positive electrode film.

[0159] The graphitization degree C of the positive electrode film was obtained by the ratio of the peak intensities of the G-band and D-band in the Raman spectrum. The position of the G-band peak was 1580±100 cm⁻¹. -1 Its characterization of carbon sp 2 Hybrid structure; D peak position is 1350±100 cm⁻¹ - 1 It characterizes the disordered structure of carbon, where disorder refers to the irregular arrangement of carbon atoms in the structure.

[0160] The cumulative distribution curve of graphitization degree C value refers to the curve obtained by arranging at least 100 C values ​​in ascending order, with graphitization degree as the horizontal axis and the cumulative percentage as the vertical axis. 50 This represents the C value corresponding to a cumulative percentage of 50% on the vertical axis of the cumulative distribution curve of graphitization degree C. The median C value of graphitization degree. 50Compared to point values, it can reflect the overall graphitization degree of particles in the positive electrode film, i.e., the degree of slippage; compared to the mean value, it can reduce the influence of extreme values ​​during the test and improve the confidence of the test results.

[0161] Those skilled in the art can control the degree of graphitization of active material particles using any known process. For example, adjusting the carbon source, sintering temperature, sintering time, sintering pressure, and sintering atmosphere can all achieve adjustments to the degree of graphitization of active material particles.

[0162] In some embodiments, the median C of the graphitization degree C in the cumulative distribution curve of the positive electrode film obtained in laser microscopy confocal Raman spectroscopy instrument scanning mode is... 50 The value can be selected from 1.0, 1.01, 1.02, 1.03, 1.04, 1.05, 1.06, 1.07, 1.08, 1.09, 1.1, 1.11, 1.12, 1.13, 1.14, 1.15, 1.16, 1.17, 1.18, 1.19, 1.20, or any value range between the two.

[0163] In the cumulative distribution curve of graphitization degree C obtained by laser microscopy confocal Raman spectroscopy in instrument scanning mode, the median C of graphitization degree is... 50 Within the aforementioned range, the sliding rearrangement between particles can be promoted, thereby increasing the compaction density of the electrode sheet. This reduces the content of large particles in the positive electrode film, which helps to reduce the rebound phenomenon caused by excessive large particles in the film while maintaining the high capacity of the pouch cell. It further reduces the probability of contact and short circuit between the negative and positive electrode films in the electrode sheet, reduces the amount of gas generated by the electrolyte due to high-temperature decomposition, thereby reducing the probability of encapsulation failure near the current lead-out components, improving the cycle performance of the pouch cell, and giving the battery device good safety performance and high overall capacity.

[0164] In some implementations, the median B of the coating value B in the cumulative distribution curve of the positive electrode film obtained in laser microscopy confocal Raman spectroscopy instrument scanning mode is... 50 The value is 0.30-0.60, where the coating value B is I. P / I D , where I P This indicates that the Raman spectrum is at 948±100 cm⁻¹ -1 The intensity of the P peak at I D This indicates that the Raman spectrum is at 1350±100 cm⁻¹ -1 The intensity of peak D at that location.

[0165] The cumulative distribution curve of the coating value (B-value) is obtained by arranging at least 100 B-values ​​in ascending order, with the coating value on the horizontal axis and the cumulative percentage on the vertical axis. To reduce the influence of extreme coating values ​​caused by non-particle regions in the positive electrode film on the test results, the median coating value (B-value) is used. 50 Evaluate the density of the carbon material layer on the positive electrode active material. B 50 The B value is the B value corresponding to the cumulative number of values ​​on the vertical axis of the cumulative distribution curve of the coverage value B value when the cumulative number accounts for 50%.

[0166] In this application, the coating value (B-value) of the positive electrode film can be obtained by scanning with a laser confocal microscopy (LCM) spectrometer. Specifically, a high-precision Renishaw laser confocal microscopy (LCM) spectrometer is used, with an excitation wavelength of 532 nm. A suitable amount of the positive electrode film is scanned on its surface or along a section of the electrode thickness. The scanning area is 45 μm × 45 μm, divided into 10 × 10 grids, with grid vertices as test points, a step size of 5 μm, and a total of 100 scan points. This yields the B-values ​​at different locations and the cumulative distribution curve of the B-values ​​in the scanned area. The positive electrode film in this application can be either freshly prepared or obtained from disassembly from a battery. Positive electrode films obtained from disassembly inevitably have residual electrolyte salt particles on their surface. To improve testing accuracy, it is preferable to perform a surface scan on a section of the positive electrode film along the electrode thickness to characterize the coating value.

[0167] The coating value B of the positive electrode film was obtained by the ratio of the peak intensities of the P-band and D-band in the Raman spectrum, with the P-band located at 948±100 cm⁻¹. -1 Its characterization of phosphate PO4 3- Structure; D peak position is 1350±100cm -1 , is one of the characteristic peaks of carbon materials, and its characterization of sp 2 Defects or disordered structures in the hybrid carbon atom lattice. During the test, an excitation wavelength of 532 nm was selected, and the test depth was shallow, only covering the particle surface. Therefore, in the test results obtained by laser microscopy confocal Raman spectroscopy in the instrument scanning mode, the carbon structure peak showed a higher intensity than the phosphate structure peak.

[0168] Those skilled in the art can control the coating value of active material particles using any known process. For example, adjusting the carbon source type, carbon source addition amount, sintering temperature, sintering time, sintering pressure, and sintering atmosphere can all achieve adjustments to the coating value of the active material particles. The coating value (B-value) reflects the density of the carbon material layer on the surface of lithium transition metal phosphate particles. The denser the carbon material layer, the lower the relative intensity of the phosphate structure detected in the Raman spectrum, and the smaller the coating value (B-value) of the cathode film.

[0169] In some embodiments, the positive electrode film further includes a coating layer disposed on at least a portion of the surface of the lithium-containing transition metal phosphate particles, wherein the median B of the coating value B in the cumulative distribution curve of the positive electrode film obtained in laser microscopy confocal Raman spectroscopy instrument scanning mode is... 50 The value can be selected from 0.3, 0.31, 0.32, 0.33, 0.34, 0.35, 0.355, 0.36, 0.368, 0.369, 0.37, 0.38, 0.39, 0.4, 0.41, 0.42, 0.43, 0.44, 0.446, 0.45, 0.456, 0.46, 0.47, 0.48, 0.49, 0.5, 0.51, 0.52, 0.53, 0.54, 0.55, 0.56, 0.57, 0.58, 0.59, 0.6, or any value range between the two.

[0170] The median B of the coating value of the positive electrode film 50 Within the aforementioned range, the carbon material layer of the positive electrode active material is relatively dense and uniform, which is beneficial to improving the slip uniformity of the positive electrode film during the rolling process and reducing stress concentration in the positive electrode film. In addition, thanks to the dense and uniform carbon material layer, large particles in the positive electrode film are more likely to slip during the compaction process, thereby reducing stress concentration at large particles in the positive electrode film, reducing rebound caused by stress release at large particles during cycling, further reducing the probability of contact and short circuit between the negative electrode film and the positive electrode film in the electrode sheet, reducing the amount of gas generated by electrolyte decomposition at high temperature, thereby reducing the probability of encapsulation failure near the current lead-out component. On the basis of the high capacity of the soft-pack battery cell, the cycle performance of the soft-pack battery cell is further improved, and the battery device has good safety performance and high overall capacity.

[0171] In some embodiments, the lithium transition metal phosphate particles include magnesium, and the magnesium content is 1000ppm-3000ppm based on the total mass of the lithium transition metal phosphate particles in the positive electrode film.

[0172] In some embodiments, the lithium transition metal phosphate particles include magnesium, and the magnesium content is 1000ppm-2000ppm based on the total mass of the lithium transition metal phosphate particles in the positive electrode film.

[0173] The types and contents of elements in lithium transition metal phosphate particles in the positive electrode film can be tested using any method known in the art. As an example, inductively coupled plasma atomic emission spectrometry (ICP-AES) was used to test the magnesium content, referring to Appendix C of GB / T 33822-2017.

[0174] In some embodiments, based on the total mass of lithium transition metal phosphate particles in the positive electrode film, the mass content of magnesium can be selected as 1000ppm, 1100ppm, 1200ppm, 1400ppm, 1500ppm, 1600ppm, 1700ppm, 1800ppm, 1900ppm, 2000ppm, 2100ppm, 2200ppm, 2300ppm, 2400ppm, 2500ppm, 2600ppm, 2700ppm, 2800ppm, 2900ppm, 3000ppm, or any value range between the two.

[0175] Doping magnesium in positive electrode active materials can increase the Fe content in lithium iron phosphate materials. 3+ / Fe 2+ The concentration of coexisting states creates more electron-hole vacancies, thereby improving the electronic conductivity of the material. It also helps to broaden the lithium-ion diffusion channels, reduce Li+ migration resistance, and improve the rate performance of the soft-pack battery cells.

[0176] In some implementations, the mass content of titanium is 500ppm-8000ppm based on the total mass of lithium transition metal phosphate particles in the positive electrode film.

[0177] In some embodiments, the mass content of titanium is 1000ppm-3000ppm based on the total mass of lithium transition metal phosphate particles in the positive electrode film.

[0178] The types and contents of elements in lithium transition metal phosphate particles in the positive electrode film can be tested using any method known in the art. As an example, inductively coupled plasma atomic emission spectrometry (ICP-AES) was used to test the titanium content, referring to Appendix C of GB / T 33822-2017.

[0179] In some embodiments, based on the total mass of lithium transition metal phosphate particles in the positive electrode film, the mass content of titanium can be selected as 500ppm, 600ppm, 700ppm, 800ppm, 900ppm, 1000ppm, 1100ppm, 1200ppm, 1400ppm, 1500ppm, 1600ppm, 1700ppm, 1800ppm, 1900ppm, 2000ppm, 2100ppm, 2200ppm, 2300ppm, 2400ppm, 2500ppm, 2600ppm, 2700ppm, 2800ppm, 2900ppm, 3000ppm, 3500ppm, 4000ppm, 4500ppm, 5000ppm, 5500ppm, 6000ppm, 6500ppm, 7000ppm, 7500ppm, 8000ppm, or any value range between the two.

[0180] Introducing titanium into lithium transition metal phosphate particles requires adding a titanium source during the preparation of the cathode active material. Titanium sources are often inert materials, and their adhesion to the surface of the lithium transition metal phosphate particles reduces reactivity and particle size growth. Increasing the graphitization degree of the cathode active material often requires higher sintering temperatures or longer sintering times, but this also increases the particle size in the cathode film, increases stress concentration in the cathode film, and increases the rebound of the electrode during cycling. In this embodiment, by adding a high content of titanium to the lithium transition metal phosphate particles, the reactivity of the raw materials for synthesizing the cathode active material is reduced. This allows the cathode active material to achieve a high degree of graphitization while controlling the proportion of large particles, reducing stress concentration in the cathode film, and improving the rebound phenomenon caused by stress concentration at large particles. This further improves the cycle performance of the pouch cell while maintaining good capacity.

[0181] Meanwhile, the doping of titanium in the positive electrode active material is beneficial for inducing lattice distortion, reducing Li-O bond energy, increasing lithium-ion transport rate, and improving the kinetic performance of the battery. The uneven diffusion of lithium ions in the positive electrode film often involves a significant lithium-ion concentration gradient. This application's embodiments improve the solid-phase transport rate of the positive electrode active material by adding a high content of titanium to lithium-containing transition metal phosphate particles, thereby addressing the kinetic issues of the single-cell pouch battery.

[0182] In some implementations, the vanadium content is 500 ppm to 5000 ppm based on the total mass of lithium transition metal phosphate particles in the positive electrode film.

[0183] The types and contents of elements in lithium transition metal phosphate particles in the positive electrode film can be tested using any method known in the art. As an example, inductively coupled plasma atomic emission spectrometry (ICP-AES) is used to test the vanadium content, referring to Appendix C of GB / T 33822-2017.

[0184] In some embodiments, the vanadium content can be selected as 500ppm, 600ppm, 700ppm, 800ppm, 900ppm, 1000ppm, 1100ppm, 1200ppm, 1400ppm, 1500ppm, 1600ppm, 1700ppm, 1800ppm, 1900ppm, 2000ppm, 2100ppm, 2200ppm, 2300ppm, 2400ppm, 2500ppm, 2600ppm, 2700ppm, 2800ppm, 2900ppm, 3000ppm, 3500ppm, 4000ppm, 4500ppm, or 5000ppm, based on the total mass of lithium transition metal phosphate particles in the positive electrode film.

[0185] In some implementations, the vanadium content is 500 ppm to 3000 ppm based on the total mass of lithium transition metal phosphate particles in the positive electrode film.

[0186] Vanadium in the positive electrode film can be in multiple valence states, including +5 vanadium (V5). 5+ Vanadium (V+3) can be doped into phosphorus sites. Due to its large radius, it can cause lattice distortion, expand the diffusion channels of lithium ions, thereby improving the ionic conductivity of the positive electrode active material and enhancing the kinetic performance of the battery; 3+ Vanadium can be doped into transition metal sites, generating lithium vacancies through charge compensation, thereby improving the electronic conductivity of the positive electrode active material. Furthermore, the increased uniformity of vanadium distribution in lithium-containing transition metal phosphate particles helps to further improve the kinetic performance and reaction uniformity of the positive electrode film, thus further enhancing the kinetic and cycle performance of the pouch cell.

[0187] Vanadium content within the aforementioned range helps improve the kinetic performance of the positive electrode and the lithium transition metal phosphate battery. Simultaneously, the synergistic effect of titanium, vanadium, magnesium, and carbon nanotubes in the positive electrode film helps form a good three-dimensional network, further improving the electronic and ionic conductivity of the positive electrode film, thereby further enhancing the kinetic performance of the lithium transition metal phosphate pouch cell.

[0188] In some embodiments, the compaction density of the positive electrode sheet of a single pouch cell in its fully discharged state is 2.3 g / cm³. 3-2.6g / cm 3 .

[0189] In this application, the fully discharged state refers to the state after the battery is placed in a 25°C oven environment, left to stand for 2 hours, and the battery temperature is maintained at 25°C, and then discharged at a constant current of 1 / 3C to 2.5V and then discharged at a constant current of 0.1C to 2.0V.

[0190] The compaction density of the positive electrode sheet can be tested using methods known in the art. As an example, the battery is placed in a 25°C oven environment and left to stand for 2 hours. After the battery temperature is maintained at 25°C, the battery is discharged at a constant current of 1 / 3C to 2.5V and then discharged at a constant current of 0.1C to 2.0V. The battery is then disassembled to obtain the positive electrode sheet. The residual electrolyte is treated with dimethyl carbonate solvent, the electrode sheet is dried, and it is cut into small circular pieces with an area of ​​S. The mass of the circular pieces is obtained as W1, and the thickness of the positive electrode sheet is measured using a micrometer. Then, the positive electrode film layer of the weighed electrode sheet is wiped off, the mass of the current collector is weighed and recorded as W2, and the thickness of the current collector is measured using a micrometer. Then, the compaction density of the positive electrode sheet is PD=(W1-W2) / [(T1-T2)×S].

[0191] In some embodiments, the compaction density of the positive electrode sheet of a single pouch cell in its fully discharged state can be selected as 2.3 g / cm³. 3 2.31 g / cm 3 2.32 g / cm 3 2.33 g / cm 3 2.34 g / cm 3 2.35g / cm 3 2.36 g / cm 3 2.37 g / cm 3 2.38g / cm 3 2.39 g / cm 3 2.40 g / cm 3 2.41 g / cm 3 2.42 g / cm 3 2.43 g / cm 3 2.44 g / cm 3 2.45g / cm 3 2.46 g / cm 3 2.47 g / cm 3 2.48 g / cm 3 2.49 g / cm 3 2.50g / cm 3 2.51g / cm 3 2.52g / cm 3 2.53g / cm 3 2.54 g / cm3 2.55g / cm 3 2.56 g / cm 3 2.57g / cm 3 2.58g / cm 3 2.59g / cm 3 2.60g / cm 3 Or the range of values ​​between any two.

[0192] When a single pouch cell is fully discharged, the compaction density of the positive electrode sheet is less than 2.3 g / cm³. 3 When the battery is in a state of insufficient interparticle connection, it not only fails to achieve ideal capacity performance, but also hinders the formation of electron conduction networks and lithium-ion transport channels, significantly increasing the battery's internal resistance and leading to increased ohmic heat generation. Furthermore, when the compaction density of the positive electrode sheet of a single battery cell in a fully discharged state exceeds 2.6 g / cm³, the battery will not achieve the desired capacity performance. 3 If the porosity of the positive electrode is too low, it will hinder lithium-ion diffusion and increase the electrochemical heat generation of the battery. Controlling the compaction density of the positive electrode within the above range is beneficial to improving the ohmic heat generation and electrochemical heat generation of the battery, thereby balancing the capacity and cycle performance of the pouch cell.

[0193] In some implementations, the porosity of the positive electrode film is 14%-22%.

[0194] The porosity of the positive electrode film can be tested as follows: Import the cross-sectional SEM image of the positive electrode film along the thickness direction obtained as described above into ImageJ software. Select the line tool and use a line to mark the length of the scale bar in the image. Click "Analyze Set Scale" and set the scale parameters in the software according to the scale bar length in the image. Select the rectangle tool and select the part of the image outside the scale bar area. Use "Image Duplicate" to copy the selected area and use "Image Type 8bit" to adjust the image format. Select "Analyze Set Measurements" and choose the following 5 options: "Area", "Mean gray value", "Area Fraction", "Limit to threshold", and "Feret's diameter". Select 3 for "Decimal places". Then select "Image" - "Adjust" - "Threshold" in sequence and set 0 and 100 in the "Threshold" box. You can then use the Analyze-Measure function to export the porosity data from the cross-sectional SEM image. Export using "Image" - "Overlay" - "Flatten" to obtain a pore image; click "Apply" in "Threshold", then click "Analyze" - "Analyze Particles", check the four columns on the left to obtain pore statistics.

[0195] It is understood that in the embodiments of this application, "pores" in the cross-section of the positive electrode film are identified by image color difference and threshold. These "pores" are not pore data obtained from the degassing test, but are mainly used to characterize the cross-sectional area between particles in the cross-section of the positive electrode film. This method is superior to the degassing method because the porosity obtained by the degassing method is related to the pores between particles and the pores in the carbon material on the surface of the lithium iron phosphate particles, thus failing to objectively reflect the pores between particles.

[0196] In some embodiments, the porosity of the positive electrode film can be selected as 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, or any value range between the two.

[0197] Porosity within the above-mentioned range of the positive electrode film layer is beneficial to improving the electrolyte retention characteristics, improving the ion diffusion of the large-particle positive electrode film layer with a certain area ratio, and improving the dynamic performance of the soft-pack battery cell.

[0198] In some embodiments, the positive electrode film layer further includes a conductive agent, which includes carbon nanotubes, and the carbon nanotubes include one or more of single-walled carbon nanotubes, few-walled carbon nanotubes, and multi-walled carbon nanotubes. The mass content of carbon nanotubes is 0.05%-2.5% based on the mass of the positive electrode film layer.

[0199] In this application, the term "carbon nanotube" refers to a structure composed of carbon atoms arranged in sp... 2 Graphene sheets, formed by hybrid bonding, are rolled up to form nanomaterials with several to dozens of coaxial hollow cylindrical layers. Their diameters typically range from several to tens of nanometers, while their lengths can vary from micrometers to centimeters, exhibiting a high aspect ratio. Based on the number of layers, graphene sheets can be classified into: single-walled carbon nanotubes (SWCNTs), few-walled carbon nanotubes (FWCNTs), and multi-walled carbon nanotubes (MWCNTs). Carbon nanotubes possess excellent electrical conductivity and high elastic modulus.

[0200] In some embodiments, based on the mass of the positive electrode film, the mass content of carbon nanotubes can be selected as 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, or any value range between the two.

[0201] Carbon nanotubes have a high aspect ratio, which facilitates the bonding of multiple positive electrode particles in the thickness direction, forming a long-range conductive path while increasing the binding force between particles. This reduces local polarization and even lithium plating problems in pouch cell during cycling, thus improving the cycle life of pouch cell. Furthermore, through the binding effect, it reduces the rebound phenomenon of large particles in the positive electrode film, further reducing the probability of contact and short circuit between the negative electrode film and the positive electrode film in the electrode sheet. It also reduces the amount of gas generated by electrolyte decomposition at high temperature, thereby reducing the probability of encapsulation failure near the current lead-out components, further improving the cycle performance of pouch cell, and giving the battery device good safety performance.

[0202] Having a carbon nanotube content within the above range helps reduce the probability of excessive agglomeration of the conductive agent due to excessive carbon nanotube content, allowing it to be evenly distributed in the positive electrode film layer. This is beneficial for further improving the cycle performance of the pouch cell and enhancing the safety performance of the battery device.

[0203] In some embodiments, the conductive agent further includes conductive carbon black, the mass content of which is 0.05%-2.5% based on the mass of the positive electrode film.

[0204] In some embodiments, based on the mass of the positive electrode film, the mass content of conductive carbon black can be selected as 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, or any value range between the two.

[0205] Conductive carbon black, with its small size, adheres to the surface of positive electrode particles and fills the gaps between them, forming dense, dot-like conductive contacts. Its combination with carbon nanotubes balances long-range and short-range conductivity, further improving the conductive network within the positive electrode film. Simultaneously, the conductive agent's large specific surface area facilitates liquid absorption and retention, reducing electrolyte extrusion caused by high expansion forces during long cycles and improving the cycle life of individual pouch cells.

[0206] When the mass content of carbon nanotubes and conductive carbon black is within the above range, it can effectively alleviate the aggregation of carbon nanotubes and form a good conductive network structure, thereby effectively reducing the stress concentration of the positive electrode film and improving the liquid retention rate of the positive electrode film during long-term cycling. This further reduces the risk of electrode film detachment and polarization, improves the dynamic performance of the pouch cell, and enhances the cycle life of the pouch cell.

[0207] In some embodiments, the total area of ​​the agglomerated region of the conductive agent is 0.2%-6.0%, optionally 1.5%-5.0%, based on the total area of ​​the cross-section of the positive electrode film along the thickness direction of the electrode sheet; the agglomerated region of the conductive agent includes carbon nanotubes and conductive carbon black.

[0208] In this application, the area ratio of the conductive agent agglomeration region, based on the total area of ​​the cross-section of the positive electrode film layer along the electrode thickness direction, can be tested using the following method. A similar method to that described above is used to observe the cross-section of the positive electrode film layer along the electrode thickness direction using a scanning electron microscope (SEM), and the area of ​​the conductive agent agglomeration region in the SEM image is measured at 3kx magnification. Since the conductive agent is generally a carbon-based material, such as conductive carbon black or carbon nanotubes, aggregated conductive agent can be seen under high magnification in the SEM. The conductive agent agglomeration region often appears black and agglomerated compared to other areas in the positive electrode film layer. Using image analysis software, the conductive agent agglomeration region refers to the area in the SEM image where the conductive agent is clearly aggregated and appears black. Specifically, the scanning electron microscope (SEM) image at 3kx magnification is imported into ImageJ. Black conductive agent agglomeration regions with a Feret value greater than or equal to 2μm are selected, and the sum of the areas of these selected regions is recorded as the area of ​​the conductive agent agglomeration region. The area ratio of the conductive agent agglomeration region is the ratio of its area to the total area of ​​the imported SEM image. Three randomly selected, non-overlapping SEM images are used, and the average of these ratios is calculated as the "area ratio of the conductive agent agglomeration region based on the total area of ​​the cross-section along the electrode thickness direction of the positive electrode film."

[0209] In some embodiments, based on the total area of ​​the cross-section of the positive electrode film along the electrode thickness direction, the area percentage of the conductive agent agglomeration region can be selected as 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, or 2.7%. 2.8%, 2.9%, 3.0%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4.0%, 4.1%, 4.2%, 4.3%, 4.4%, 4.5%, 4.6%, 4.7%, 4.8%, 4.9%, 5.0%, 5.1%, 5.2%, 5.3%, 5.4%, 5.5%, 5.6%, 5.7%, 5.8%, 5.9%, 6.0%, or any range between two of these values.

[0210] Based on the total area of ​​the cross-section of the positive electrode film along the thickness direction of the electrode sheet, the total area ratio of the agglomeration region of the conductive agent within the above range indicates that the conductive agent in the positive electrode film is uniformly dispersed and easy to form a uniform conductive network, which is beneficial to reduce the local polarization and even lithium plating problems generated by the soft-pack battery cells during cycling.

[0211] Meanwhile, research shows that large particles in lithium transition metal phosphates are prone to rebound. When the agglomeration area of ​​the conductive agent is within the above range, the uniform distribution of the conductive agent can suppress the rebound of lithium transition metal phosphate particles, form mechanical constraints on the particles and even the film layer, improve the cohesion of the film layer, reduce the damage of the SEI film and film layer during the rebound process, and improve the cycle life of the soft-pack battery cell.

[0212] In some embodiments, the positive electrode film layer further includes a conductive agent, and the area of ​​the agglomerated region of the conductive agent accounts for 1.5%-5.0% based on the total area of ​​the cross section of the positive electrode film layer along the thickness direction of the electrode sheet.

[0213] The aggregation area of ​​the conductive agent within the above range is beneficial to further improve the cycle life of the soft-pack battery cell.

[0214] In some embodiments, the agglomeration regions of the conductive agent include carbon nanotubes and conductive carbon black.

[0215] Researchers have discovered that carbon nanotubes, due to their high surface energy, are prone to aggregation, leading to uneven dispersion in the positive electrode film and hindering the formation of an effective carbon nanotube network structure. Conductive carbon black, with a surface energy similar to that of carbon nanotubes, can adsorb onto the carbon nanotube surface, forming a physical barrier that increases the resistance to aggregation, reduces direct contact between carbon nanotubes, and thus inhibits aggregation, improving the uniformity of carbon nanotube distribution in the positive electrode film. This helps improve the conductivity of the positive electrode film, enhancing the battery's kinetic performance; it also helps leverage the binding effect of carbon nanotubes on the positive electrode film, reducing the risk of film detachment and further improving the battery's kinetic performance and cycle life. Furthermore, the aggregation of carbon nanotubes in the conductive agent aggregation region can also lead to local blockage of ion transport pathways in this region. The addition of conductive carbon black can improve the lithium-ion transport capacity in this region, reduce local polarization, and further improve the cycle stability of individual pouch cell cells.

[0216] In some implementations, the thickness of the positive electrode film on one side is 70 μm-120 μm.

[0217] It should be noted that the positive electrode film layer contains lithium transition metal phosphate particles, but the positive electrode film layer does not only refer to the positive electrode active material layer. Other film layers that are connected to the positive electrode active material layer and are difficult to distinguish, such as the undercoat layer and the liquid retention layer, are all collectively referred to as the positive electrode film layer.

[0218] The thickness of the positive electrode film can be measured using any method known in the art. As an example, the thickness of the positive electrode film in a cross-section along the thickness direction of the positive electrode sheet is measured using a scanning electron microscope. Measurements are taken at three randomly selected locations, and the average value is taken as the thickness of the positive electrode film.

[0219] In some embodiments, the thickness of one side of the positive electrode film can be selected as 70μm, 71μm, 72μm, 73μm, 74μm, 75μm, 76μm, 77μm, 78μm, 79μm, 80μm, 81μm, 82μm, 83μm, 84μm, 85μm, 86μm, 87μm, 88μm, 89μm, 90μm, 91μm, 92μm, 93μm, 94μm, 95μm, 96μm. m, 97μm, 98μm, 99μm, 100μm, 101μm, 102μm, 103μm, 104μm, 105μm, 106μm, 107μm, 108μm, 109μm, 110μm, 111μm, 112μm, 113μm, 114μm, 115μm, 116μm, 117μm, 118μm, 119μm, 120μm or any numerical range in between.

[0220] The specific capacity of lithium-containing transition metal phosphate particles is relatively low. Studies have shown that when the single-sided thickness of the positive electrode film is less than 70 μm, the capacity of the battery cell is difficult to meet market demand. A single-sided thickness of the positive electrode film within the aforementioned range is beneficial for improving the capacity of pouch cell batteries. However, increasing the thickness of the positive electrode film leads to longer electron and ion transport paths, increased resistance of the positive electrode film, and increased ohmic and electrochemical heat generation on the positive electrode. Controlling the thickness of the positive electrode film within a reasonable range is beneficial for improving the capacity of pouch cell batteries and further improving their cycle performance.

[0221] In some implementations, the thickness of the positive electrode film on one side is 90 μm-120 μm.

[0222] The thickness of the positive electrode film on one side within the above range is beneficial to further improve the capacity of the individual soft-pack battery cells, thereby increasing the overall capacity of the battery device.

[0223] In some implementations, the thickness of the positive electrode film on one side is 100 μm-120 μm.

[0224] Increasing the thickness of the positive electrode film on one side is beneficial to improving the capacity of the pouch cell. The applicant found that when the thickness of the positive electrode film on one side is greater than or equal to 100 μm, the phenomenon of particle rebound in the positive electrode film is more serious. The embodiments of this application effectively alleviate the serious rebound of the thick coating film during the cycle of the pouch cell. The pouch cell has good cycle performance while maintaining a high capacity.

[0225] In some embodiments, as shown in FIG5, the length dimension L0 of the soft-pack battery cell is 500mm-1250mm; the width dimension W0 is 100mm-150mm; and the thickness dimension H0 is 14mm-22mm.

[0226] The dimensions of the soft-pack battery cells in this application embodiment are within the above-mentioned range, which is beneficial for achieving better capacity in the battery cells and improving the overall capacity of the battery device.

[0227] In some implementations, L0 can be selected as 500mm, 510mm, 520mm, 530mm, 540mm, 550mm, 560mm, 570mm, 580mm, 590mm, 600mm, 610mm, 620mm, 630mm, 640mm, 650mm, 660mm, 670mm, 680mm, 690mm, 700mm, 710mm, 720mm, 750mm, 800mm, 850mm, 900mm, 950mm, 1000mm, 1050mm, 1100mm, 1150mm, 1200mm, 1250mm, or any value range between the two.

[0228] In some implementations, W0 can be selected as 100mm, 110mm, 120mm, 130mm, 140mm, 150mm or any value range between the two.

[0229] In some implementations, H0 can be selected as 14mm, 15mm, 16mm, 17mm, 18mm, 19mm, 20mm, 21mm, 22mm or any value range between the two.

[0230] In some implementations, the length dimension L0 of the pouch cell satisfies: 500mm≤L0≤650mm.

[0231] When the length dimension L0 of a pouch cell satisfies 500mm≤L0≤650mm, the pouch cell has a shorter length, which helps to shorten the electron transport path, reduce the internal resistance of the battery, and thus reduce the heat generation of the battery. Especially under fast charging conditions, it can reduce the uneven temperature rise and uneven current density along the length of the electrode, and improve the cycle performance of the pouch cell.

[0232] In some implementations, the length dimension L0 of the pouch cell satisfies: 900mm≤L0≤1250mm.

[0233] When the length dimension L0 of a pouch cell satisfies 900mm≤L0≤1250mm, the significantly increased cell size is more conducive to module-free integration, enabling the cell to be directly integrated into the battery device, significantly improving space utilization, thereby increasing the overall capacity of the battery device in the same volume, while reducing the number of structural components and improving the overall capacity of the battery device.

[0234] In some embodiments, referring to FIG8, the packaging bag 201 includes an encapsulation layer 223, a metal layer 222, and a protective layer 221 stacked sequentially from the inside of the battery cell to the outside of the battery cell. The metal layer 222 includes aluminum; the encapsulation layer 223 and the protective layer 221 include resin material.

[0235] In some implementations, the packaging bag is sealed by melting and bonding the sealing layers together.

[0236] In some embodiments, an encapsulation is formed between the packaging bag and the current lead by adhesive. It is understood that this adhesive may be formed by melting the encapsulation layer resin inside the packaging bag, or it may be formed together with the packaging bag and other applied adhesives.

[0237] Packaging bag materials containing the above-mentioned components have high elongation, which helps to improve the space utilization of battery cells, thereby increasing the energy density and capacity of battery cells. However, the composite material composed of aluminum and resin materials has poor thermal conductivity, resulting in low heat dissipation efficiency of pouch battery cells. Therefore, if the area ratio of large particles in the positive electrode film is too high, it will cause severe rebound phenomenon in the positive electrode film, leading to SEI film damage and film cracking. This can easily lead to misalignment between the positive and negative electrode plates and the separator, increasing the risk of local short circuits in the battery. Consequently, it will lead to increased local current density and temperature, accelerating electrolyte decomposition and increasing gas production, thus exacerbating the probability of encapsulation failure near the current lead. The embodiments of this application use the above-mentioned packaging bag and control the area ratio of large particles in the positive electrode film within a suitable range. The pouch battery cells have high capacity and good safety and cycle performance, and the battery device has high overall capacity and good safety performance.

[0238] In some embodiments, the encapsulation layer comprises a polypropylene layer; the protective layer comprises one or more of nylon and polyethylene terephthalate (PET). In some embodiments, the encapsulation layer comprises a polypropylene (PP) layer and a modified polypropylene (PPa) layer disposed between the polypropylene (PP) layer and the metal layer; the protective layer comprises one or more of nylon and polyethylene terephthalate (PET).

[0239] In this article, modified polypropylene refers to functionalized materials that optimize the properties of ordinary polypropylene (PP) through chemical or physical means, including but not limited to grafting maleic anhydride onto the polypropylene molecular chain, introducing ethylene monomers to copolymerize with propylene, blending polypropylene with polyolefin elastomers or EPDM rubber, and adding nano-inorganic particles (such as nano-silica). Different modification methods are beneficial for specifically improving the heat-sealing properties, chemical resistance, adhesion and mechanical strength of the material.

[0240] Modified polypropylene further improves the electrolyte corrosion resistance and bonding strength of the packaging bag. This encapsulation layer helps reduce interface leakage caused by insufficient heat sealing strength. The outer protective layer has excellent mechanical properties, which can buffer mechanical impact during assembly, reduce the risk of encapsulation failure of soft-pack battery cells, improve the safety performance of soft-pack battery cells, and thus improve the reliability of battery devices.

[0241] In some embodiments, the modified polypropylene (PPa) layer comprises maleic anhydride-grafted polypropylene.

[0242] Studies have shown that the main encapsulation failure sites near the current lead are the interfacial delamination between the polypropylene layer and the metal layer under high temperatures. The carboxyl groups (—COOH) and anhydride groups (—CO—O—CO—) of maleic anhydride can chemically bond with the hydroxyl groups (—OH) or alumina (Al2O3) on the aluminum foil surface, while simultaneously maintaining molecular chain entanglement with the polypropylene matrix. This helps to further improve the peel strength between the encapsulation layer and the metal layer, reducing the probability of delamination between the encapsulation layer and the metal layer under heat flow, lowering the risk of encapsulation failure in individual pouch cells, further improving the safety performance of pouch cell pouch cells, and enhancing the reliability of the battery device.

[0243] In some embodiments, the packaging bag is heat-sealed at 180°C-220°C.

[0244] The heat sealing temperature of the packaging bag is within the above range, which helps to enhance the interfacial bonding strength, reduce the probability of delamination between the encapsulation layer and the metal layer during battery cycling, reduce the risk of encapsulation failure of soft-pack battery cells, improve the safety performance of soft-pack battery cells, and improve the reliability of battery devices.

[0245] In some embodiments, the packaging bag is heat-sealed at 200°C-210°C.

[0246] The heat sealing temperature of the packaging bag is within the above range, which helps to further enhance the bonding strength between the encapsulation layer and the metal layer, thereby reducing the probability of delamination between the encapsulation layer and the metal layer during battery cycling, reducing the risk of encapsulation failure of soft-pack battery cells, improving the safety performance of soft-pack battery cells, and thus improving the reliability of battery devices.

[0247] In some embodiments, as shown in FIG3, thermally conductive structural adhesive 4 is provided between the support plate 11 of the housing and the second surface 22 of the soft-pack battery cell 2.

[0248] The thermally conductive structural adhesive of this application embodiment has good thermal conductivity and mechanical properties, which is beneficial for heat transfer from the soft-pack battery cell to the support plate for heat dissipation, thereby improving the cycle performance and safety performance of the soft-pack battery cell.

[0249] In some embodiments, as shown in FIG4, a thermal management component 3 is provided between the support plate 11 of the housing and the second surface 22 of the soft-pack battery cell 2. The thermal management component 3 is used to regulate the temperature of the soft-pack battery cell 2, and a thermally conductive structural adhesive 4 is provided between the thermal management component 3 and the second surface 22 of the soft-pack battery cell 2.

[0250] The heat from a single pouch battery cell can be efficiently dissipated through thermal management components, which helps to further improve the cycle performance and safety performance of the pouch battery cell.

[0251] In some embodiments, at 85°C, the thermal conductivity of the thermally conductive structural adhesive is greater than or equal to 0.4 W / (m·K), optionally 0.4 W / (m·K)-1.2 W / (m·K), and further optionally 0.8 W / (m·K)-1.2 W / (m·K).

[0252] The thermal conductivity of the thermally conductive structural adhesive at 85°C can be tested using methods known in the art. As an example, the transient hot disk method (Hot Disk) can be used, according to ISO 22007-2. A temperature probe with a self-heating function is placed under a sample disc with a diameter greater than 30 mm and a thickness greater than 2 mm. Standard weights from Hengzhong Company are used to press down on the sample disc. During the test, a constant heating power is applied to the nickel coil of the probe, causing its temperature to rise. Since the temperature coefficient of resistance (TCR) of nickel is linear (ΔR / R0 = αΔT), the heat loss can be obtained by measuring the change in resistance, thereby determining the thermal conductivity of the sample at 85°C.

[0253] In some embodiments, the thermal conductivity of the thermally conductive structural adhesive at 85°C can be selected as 0.4 W / (m·K), 0.5 W / (m·K), 0.6 W / (m·K), 0.7 W / (m·K), 0.8 W / (m·K), 0.81 W / (m·K), 0.82 W / (m·K), 0.83 W / (m·K), 0.84 W / (m·K), 0.85 W / (m·K), 0.86 W / (m·K), 0.87 W / (m·K), or 0.88 W / (m·K). The values ​​are 0.89 W / (m·K), 0.90 W / (m·K), 0.91 W / (m·K), 0.92 W / (m·K), 0.93 W / (m·K), 0.94 W / (m·K), 0.95 W / (m·K), 0.96 W / (m·K), 0.97 W / (m·K), 0.98 W / (m·K), 0.99 W / (m·K), 1.0 W / (m·K), 1.1 W / (m·K), 1.2 W / (m·K), or any range between the two.

[0254] The thermal conductivity of the thermally conductive structural adhesive is within the above range, which has good thermal conductivity and can still conduct heat stably at high temperatures. This helps reduce the probability of thermally conductive structural adhesive failure due to temperature rise, which in turn leads to the inability of heat to be transferred from the pouch cell to the thermal management component for heat dissipation in time, resulting in heat accumulation inside the cell. This is beneficial to improving the cycle performance of the pouch cell during long-term cycling.

[0255] In some embodiments, the thermal conductivity of the thermally conductive structural adhesive is 0.8 W / (m·K)-1.0 W / (m·K) at 85°C.

[0256] If the thermal conductivity of the thermally conductive structural adhesive is within the above range, it means that the thermally conductive filler content of the thermally conductive structural adhesive is moderate, which is beneficial to balancing the thermal conductivity and mechanical properties of the thermally conductive structural adhesive.

[0257] In some embodiments, the thermally conductive structural adhesive has a storage modulus of 260MPa-1000MPa at a vibration frequency of 0.1Hz at room temperature, optionally 300MPa-800MPa, and further optionally 300MPa-600MPa.

[0258] In this application, room temperature refers to 25°C.

[0259] The storage modulus of thermally conductive structural adhesive at a vibration frequency of 0.1 Hz at room temperature can be tested using methods known in the art. As an example, dynamic thermomechanical analysis (DMA, according to IPC-TM-650 2.4.24.4) was used, employing a three-point bending test mode with a sample size of 60 mm (length) × 10 mm (width) × 2 mm (thickness). A prestress of 0.5 N–1.0 N was applied before testing, with the loading frequency set to 0.1 Hz. The temperature program was used to increase the temperature from -40 °C to 80 °C at a rate of 5 °C / min, with the default environment being air (humidity ≤30%); nitrogen protection can be used in special cases. This allows the storage modulus of the thermally conductive structural adhesive at a vibration frequency of 0.1 Hz at room temperature to be obtained.

[0260] In some embodiments, the thermally conductive structural adhesive has a storage modulus at a vibration frequency of 0.1 Hz at room temperature, which can be selected as 260 MPa, 270 MPa, 280 MPa, 290 MPa, 300 MPa, 350 MPa, 400 MPa, 450 MPa, 500 MPa, 550 MPa, 600 MPa, 650 MPa, 700 MPa, 750 MPa, 800 MPa, 850 MPa, 900 MPa, 950 MPa, 1000 MPa, or any value range between the two.

[0261] At room temperature, the energy storage modulus at a vibration frequency of 0.1 Hz is within the above range. It has good mechanical properties and can reduce the probability of creep deformation or fatigue cracking of the thermally conductive structural adhesive under long-term mechanical vibration. This reduces the probability of displacement of the soft-pack battery cell and loss of its own thermal conductivity caused by the deformation of the thermally conductive structural adhesive. The thermally conductive structural adhesive can give full play to its good thermal conductivity and further improve the cycle performance of the soft-pack battery cell in the long cycle process.

[0262] In some embodiments, the glass transition temperature of the thermally conductive structural adhesive is 50°C-60°C.

[0263] The glass transition temperature (Tg) of the thermally conductive structural adhesive can be tested using methods known in the art. As an example, dynamic thermomechanical analysis (DMA, according to IPC-TM-650 2.4.24.4) is used, and the Tg is determined by monitoring changes in the mechanical properties of the material under dynamic loads. In the test, the temperature at which the loss factor (tanδ) curve reaches its peak is the glass transition temperature (Tg). In some embodiments, the glass transition temperature of the thermally conductive structural adhesive can be selected as 50°C, 51°C, 52°C, 53°C, 54°C, 55°C, 56°C, 57°C, 58°C, 59°C, 60°C, or any value between two of these ranges.

[0264] If the glass transition temperature of the thermally conductive structural adhesive is too low, when the operating temperature of the pouch cell exceeds this glass transition temperature, the energy storage modulus of the thermally conductive structural adhesive will drop sharply, causing the adhesive to transition from a glassy state to a viscoelastic state. After softening, the adhesive cannot provide sufficient mechanical holding force, and relative displacement or interfacial debonding may occur between the pouch cell and thermal management components, reducing the thermal conductivity between the cell and the thermally conductive structural adhesive, and consequently reducing the heat dissipation efficiency of the cell. If the glass transition temperature of the thermally conductive structural adhesive is too high, at low temperatures, the adhesive remains in a glassy state, its toughness decreases, and the volume changes of the pouch cell during charging and discharging will generate stress at the interface, causing the thermally conductive structural adhesive to brittlely crack, resulting in cracks and a decrease in the heat dissipation efficiency of the cell.

[0265] When the glass transition temperature of the thermally conductive structural adhesive is within a suitable range, it is beneficial for the thermally conductive structural adhesive to fully exert its bonding and thermal conductivity, which is conducive to further improving the cycle performance of the soft-pack battery cells.

[0266] In some embodiments, the thermally conductive structural adhesive comprises a polyurethane resin and thermally conductive filler particles dispersed in the polyurethane resin; the thermally conductive filler particles comprise one or more of aluminum hydroxide particles and boron nitride particles.

[0267] Thermally conductive structural adhesives containing the above components exhibit good high-temperature resistance.

[0268] In some embodiments, the thermally conductive filler particles account for 20%-70% of the total mass of the thermally conductive structural adhesive, and optionally 45%-65%.

[0269] In some embodiments, based on the total mass of the thermally conductive structural adhesive, the mass percentage of the thermally conductive filler particles can be selected as 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, or any range between the two.

[0270] The thermally conductive filler particles in the thermally conductive structural adhesive are within the above-mentioned range, which is beneficial to improving the thermal conductivity of the thermally conductive structural adhesive and reducing the problem of insufficient resin content caused by excessive thermally conductive filler particles, which would result in poor energy storage modulus of the thermally conductive structural adhesive. The thermally conductive structural adhesive has good thermal conductivity, which is beneficial to improving the cycle performance of soft-pack battery cells.

[0271] In some embodiments, as shown in Figures 2, 3, and 4, the projection of the thermally conductive structural adhesive on the first surface does not overlap with the projection of the negative electrode sheet on the first surface.

[0272] After the battery cells are bonded to the thermally conductive structural adhesive, the adhesive may overflow. Once the battery cells are assembled into a battery device, the projection of the thermally conductive structural adhesive on the first surface does not overlap with the projection of the negative electrode sheet on the first surface. This reduces the probability of the relatively rigid thermally conductive structural adhesive and the electrode sheet directly compressing each other during battery cycling, lowering the probability of stress concentration on the battery electrode sheet caused by the thermally conductive structural adhesive, thereby reducing the adverse impact on the cycle performance of the pouch battery cells.

[0273] In some embodiments, as shown in Figures 2, 3, and 4, double-sided adhesive 5 is provided between the individual soft-pack battery cells, and a gap is provided between the double-sided adhesive 5 and the thermally conductive structural adhesive 4.

[0274] After the battery cells are bonded to the thermally conductive structural adhesive, excess adhesive may appear. The battery cells are then bonded together using double-sided adhesive. After assembling them into a battery device, a gap is created between the double-sided adhesive and the thermally conductive structural adhesive. This reduces the probability of the relatively rigid thermally conductive structural adhesive and the double-sided adhesive coming into contact with each other during battery cycling. This reduces stress concentration caused by the rigid thermally conductive structural adhesive on the double-sided adhesive between the battery cells, thereby minimizing any adverse impact on the cycle performance of the pouch battery cells.

[0275] In some embodiments, the positive current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer substrate and a metal layer formed on at least one surface of the polymer substrate. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0276] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer substrate and a metal layer formed on at least one surface of the polymer substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0277] In some embodiments, the negative electrode film layer includes a negative electrode active material. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, and hard carbon. However, this application is not limited to these materials, and other conventional materials that can be used as battery negative electrode active materials may also be used. These negative electrode active materials may be used alone or in combination of two or more.

[0278] In some embodiments, the negative electrode film layer may optionally include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0279] In some embodiments, the negative electrode film may optionally include a conductive agent. The conductive agent may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0280] In some embodiments, the negative electrode film may optionally include other additives, such as thickeners (e.g., sodium carboxymethyl cellulose (CMC-Na)).

[0281] The electrolyte acts as a conductor of ions between the positive and negative electrodes. This application does not impose specific restrictions on the type of electrolyte; it can be selected according to requirements. For example, the electrolyte can be liquid, gel, or entirely solid.

[0282] In some embodiments, the electrolyte is an electrolyte solution. The electrolyte solution includes an electrolyte salt and a solvent.

[0283] In some embodiments, the electrolyte salt may be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalate borate, lithium dioxalate borate, lithium difluorodioxalate phosphate, and lithium tetrafluorooxalate phosphate.

[0284] In some embodiments, the solvent may be selected from at least one of ethylene carbonate, propylene carbonate, methyl ethyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butyl carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, sulfolane, dimethyl sulfone, methyl ethyl sulfone, and diethyl sulfone.

[0285] In some embodiments, the electrolyte may optionally include additives. For example, additives may include negative electrode film-forming additives, positive electrode film-forming additives, and may also include additives that can improve certain battery performance, such as additives that improve battery overcharge performance, additives that improve battery high-temperature or low-temperature performance, etc.

[0286] The battery device disclosed in this application can be used in electrical devices that use the battery device as a power source or in various energy storage systems that use the battery device as an energy storage element. Besides vehicles, the battery device can also be used in, but is not limited to, mobile phones, tablets, laptops, electric toys, power tools, electric vehicles, electric cars, ships, spacecraft, etc. Electric toys can include stationary or mobile electric toys, such as game consoles, electric car toys, electric ship toys, and electric airplane toys, etc. Spacecraft can include airplanes, rockets, space shuttles, and spacecraft, etc.

[0287] Furthermore, a second aspect of this application provides an electrical device that uses a battery as a power source, the electrical device including at least one of the battery cell, battery module, or battery pack provided in this application. The battery cell, battery module, or battery pack can be used as a power source for the electrical device, or as an energy storage unit for the electrical device.

[0288] As the electrical device, a single battery cell, a battery module, or a battery pack can be selected according to its usage requirements.

[0289] Figure 9 shows an example of an electrical device. The electrical device disclosed in this application can be a gasoline-powered vehicle, a natural gas-powered vehicle, or a new energy vehicle. New energy vehicles can be pure electric vehicles, hybrid electric vehicles, or range-extended electric vehicles, etc. A battery device is installed inside the vehicle, and the battery device can be located at the bottom, front, or rear of the vehicle. The battery device can be used to power the vehicle; for example, the battery device can serve as the vehicle's operating power source. The vehicle may also include a controller and a motor. The controller is used to control the battery device to supply power to the motor, for example, for the vehicle's starting, navigation, and operating power needs. In some embodiments of this application, the battery device can not only serve as the vehicle's operating power source but also as the vehicle's drive power source, replacing or partially replacing gasoline or natural gas to provide driving power to the vehicle.

[0290] The third aspect of this application also provides an energy storage device that uses a battery device as a power source. The energy storage device can be, but is not limited to, an energy storage container, an energy storage cabinet, an energy storage power station, an energy storage battery pack, or a portable energy storage system.

[0291] Example

[0292] The following describes embodiments of this application. The embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.

[0293] Example 1

[0294] (1) Preparation of positive electrode active material

[0295] Lithium carbonate, iron phosphate, titanium dioxide, vanadium pentoxide, magnesium oxide, sucrose, glucose, and polyethylene glycol were added to deionized water and mixed in a premixing tank. The ratio of lithium carbonate to iron phosphate was such that the molar ratio of lithium to iron was 1.02:1.0. Based on the total mass of the mixed raw materials, the mass content of sucrose was 2%, the mass content of glucose was 4%, and the mass content of polyethylene glycol was 5%. After uniform mixing, a mixed raw material with a solid content of 38% was obtained.

[0296] Among them, the particle size Dv of lithium carbonate 50 The particle size is 6 μm; the morphology of the iron phosphate particles is spherical; both titanium dioxide and vanadium pentoxide are nanoparticles; the purity of sucrose is ≥98%; the moisture content of glucose is <0.5%; and the weight average molecular weight of polyethylene glycol is 1500.

[0297] The mixed raw materials were ground twice in a sand mill, coarsely ground for 1 hour and then finely ground. During the grinding process, the slurry temperature was controlled to be less than 40 degrees Celsius to obtain a mixed slurry. The particle size Dv50 of the solid particles in the mixed slurry was 0.40 μm. Spray drying was then performed to obtain a dried precursor powder, and the particle size Dv50 after drying was 55.50 μm.

[0298] The precursor powder was subjected to a two-stage heating sintering process in a nitrogen atmosphere to obtain the positive electrode active material: the temperature was increased from 25℃ to 460℃ at a heating rate of 2℃ / min (first heating stage), and held for 3 hours; the temperature was then increased from 460℃ to 780℃ at a heating rate of 5℃ / min (second heating stage), and held for 12 hours; the air volume in the heating stage was greater than that in the isothermal stage, with a ratio of 1.5:1, and the total air volume was 1350 cm³. 3 / h, after which the temperature is lowered; the lithium iron phosphate cathode active material with carbon material on the surface is obtained by air jet milling with a particle size Dv50 of 1.6μm. The total mass of the cathode active material is 1050ppm for Ti, 950ppm for V, and 1500ppm for Mg.

[0299] The Dv10, Dv50, and Dv90 mentioned above refer to data obtained through the Malvern laser scattering method.

[0300] (2) Preparation of positive electrode sheet

[0301] The above-mentioned positive electrode active material (93.9% by mass), conductive agent (2% by mass), and binder polyvinylidene fluoride (3% by mass) were mixed in the solvent N-methylpyrrolidone. Then, dispersant HNBR (1.1% by mass) was added, and the mixture was thoroughly mixed in a stirring tank. The stirring included a first stirring at 600 rpm for 30 min and a second stirring at 1600 rpm for 260 min. After dispersion, a positive electrode slurry was prepared. After the stirring process, the positive electrode slurry was conveyed to the coating process. The mass percentages of the positive electrode active material, conductive agent, binder, and dispersant were calculated based on the total mass of solids in the positive electrode slurry. The conductive agent included conductive carbon black (1.33% by mass) and single-walled carbon nanotubes (0.67% by mass). The specific surface area of ​​the conductive carbon black was 85 m². 2 / g, oil absorption value of 200ml / 100g, average length of single-walled carbon nanotubes of 30μm, specific surface area of ​​300m² 2 / g, the mass content of metallic impurities in single-walled carbon nanotubes is <1wt%;

[0302] The positive electrode slurry was transferred and coated onto a current collector aluminum foil, dried, and then hot-pressed to obtain a positive electrode film with a single-sided thickness of 104.63 μm and a compaction density of 2.36 g / cm³. 3 The positive electrode sheet. The transfer coating speed is 20 m / min.

[0303] The hot pressing process includes three hot roller pressing processes, with the hot roller pressing pressure increasing sequentially to 40 tons, 60 tons, and 80 tons. The hot roller temperature is 60℃. Before the first hot roller compaction, the electrode sheet is heated to 40℃.

[0304] The compaction density here refers to the compaction density of a single battery cell under full discharge conditions. The test method is described above.

[0305] Among them, the median C of the graphitization degree of the positive electrode film layer 50 The porosity of the positive electrode film is 17.9%; the total area of ​​the agglomerated region of the conductive agent accounts for 1.99%.

[0306] The positive electrode sheets are slit and punched into specified shapes, and then the punched positive electrode sheets are sorted by weight using a weighing and sorting machine for stacking by a stacking machine.

[0307] (3) Preparation of negative electrode sheet

[0308] Natural graphite, conductive carbon black, styrene-butadiene rubber (SBR) binder, and sodium carboxymethyl cellulose (CMC) thickener are mixed evenly in a weight ratio of 95:1:2:2 and deionized water is added. After stirring and dispersing, a negative electrode slurry is obtained. The negative electrode slurry is coated on a copper foil substrate, and after drying, compaction, slitting, and sheet forming, a negative electrode sheet is obtained.

[0309] The negative electrode sheets are slit and punched into specified shapes, and then the punched negative electrode sheets are sorted by weight using a weighing and sorting machine for stacking by a stacking machine.

[0310] (4) Diaphragm

[0311] Polyvinylidene fluoride (PVDF) was dissolved in N-methylpyrrolidone (NMP) and stirred until homogeneous. Polyethylene glycol (PEG) was then added as a pore-forming agent and thoroughly mixed to obtain an adhesive layer solution. This adhesive layer solution was applied to a base film with ceramic layers on both sides. After pre-evaporation at 80°C and drying at 110°C, the film was immersed in deionized water to dissolve the PEG, resulting in a membrane with porous adhesive layers on both sides. The base film thickness was 8 μm, the ceramic layer thickness on one side was 3 μm, and the adhesive layer thickness on one side was 1 μm.

[0312] (5) Electrolyte

[0313] In an argon atmosphere glove box (H2O < 0.1 ppm, O2 < 0.1 ppm), organic solvents dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), and ethylene carbonate (EC) are mixed evenly.

[0314] Lithium hexafluorophosphate was then added and dissolved in an organic solvent to achieve a concentration of 1.05 mol / L. Ethylene carbonate (VC) was then added and stirred until homogeneous to obtain the electrolyte of Example 1.

[0315] Based on the total mass of the electrolyte, the mass content of dimethyl carbonate is 26%, the mass content of methyl ethyl carbonate is 43.3%, the mass content of ethylene carbonate is 17.3%, and the mass content of vinylene carbonate is 0.9%.

[0316] (6) Preparation of soft-pack battery cells

[0317] The positive electrode, separator, and negative electrode are stacked in sequence using a stacking machine. The separator must effectively isolate the positive and negative electrodes to obtain a stacked battery cell. The stacked battery cell is then coated with adhesive to ensure tight containment. The coated stacked battery cell is placed in a packaging bag made of aluminum-plastic film, a soft-pack material composed of a polypropylene encapsulation layer, an aluminum foil metal layer, and a nylon protective layer. The aluminum-plastic film packaging bag is shaped and trimmed using a punching and forming machine to achieve the desired shape and size. The aluminum-plastic film is then heat-sealed at 195℃, ensuring a sealing tensile strength ≥25N / 8mm. The battery undergoes vacuum baking, settling, electrolyte injection, and sealing. Finally, the soft-pack battery is subjected to hot and cold pressing operations: hot pressing at 45℃ for 2 minutes and a pressure of 90kg / cm². 2 The cold pressing temperature was 25℃, the time was 2 minutes, and the pressure was 90 kg / cm². 2 Finally, after processes such as formation, vacuum degassing, and edge trimming, a pouch cell is obtained. The pouch cell has dimensions of 630mm in length, 130mm in width, and 20mm in thickness.

[0318] (7) Preparation of thermally conductive structural adhesive

[0319] Preparation of Component A: Polyether-modified polyol (Wanhua Chemical, grade C2004), castor oil-modified polyol (Wanhua Chemical, grade C1030D), chain extender butanediol, and thermally conductive filler aluminum hydroxide (Foshan Jingge, JAZ-176) were mixed in a mass ratio of 12:20:4:58 to obtain the first raw material. The first raw material was added to the first stirred tank and heated, stirred, and vacuumed to remove water. The water removal temperature was 120℃, the vacuum degree was -0.08MPa, the water removal time was 2h, and the rotation speed was 10rpm. After stirring and removing water, the mixture was cooled to room temperature. Then, 4 parts by mass of molecular sieve (Luoyang Jianlong, JLH-03-B), 1.5 parts by mass of silica (Evonik, grade R974), 0.2 parts by mass of catalyst dibutyltin dilaurate, and 0.3 parts by mass of yellow paste (Shanghai Jiasheng) were added to the first stirred tank and stirred and mixed evenly under vacuum to obtain Component A.

[0320] Preparation of Component B: 19 parts by weight of polyester polyol (Shanghai Jingri, DA21) were added to the second stirred tank and heated to 115℃ for dehydration for 2.5 h; then cooled to below 60℃, and 20 parts by weight of isocyanate (Wanhua Chemical, CDMDI-100L) were added. Under nitrogen protection, the mixture was heated to 65℃ at 30 rpm and stirred for 2.5 h. After the reaction, the second raw material (isocyanate prepolymer) was obtained; then, in the second stirred tank, [the following was added]... 46 parts by weight of thermally conductive filler aluminum hydroxide (Foshan Jingge, JAZ-176), 4 parts by weight of plasticizer dinonyl phthalate (Ningbo Taiying), 7 parts by weight of hydrophobic silica powder (Shenzhen Jinhaohui, GL15P3), 2.7 parts by weight of fumed silica (Jiangsu Haoneng Chemical, HN-200), 1 part by weight of molecular sieve (Luoyang Jianlong, JLH-03-B), and 0.3 parts by weight of blue paste (Shanghai Jiasheng) were mixed evenly under vacuum at 25°C for 2 hours to obtain component B.

[0321] A high-performance two-component polyurethane thermally conductive structural adhesive can be obtained by mixing component A and component B at a volume ratio of 1:1 and curing at room temperature for 7 days.

[0322] The thermally conductive structural adhesive has a thermal conductivity of 0.8 W / (m·K) at 85℃, a storage modulus of 500 MPa at room temperature and a vibration frequency of 0.1 Hz, and a glass transition temperature of 55℃.

[0323] (7) Preparation of battery device

[0324] Multiple pouch battery cells prepared above are sequentially bonded to the thermal management component along the first direction using the thermally conductive structural adhesive prepared above. After bonding, the component is moved into the housing. The housing includes a support plate, a frame, and a connecting beam to obtain the battery device. During the bonding process, the thermally conductive structural adhesive will overflow. After overflow, the projection of the thermally conductive structural adhesive on the first surface does not overlap with the projection of the negative electrode sheet in the pouch battery cell on the first surface.

[0325] The preparation methods of Examples 2-4 are basically the same as those of Example 1, except that the preparation methods of the positive electrode active material and the positive electrode sheet are adjusted, as detailed below:

[0326] Example 2

[0327] (1) Preparation of positive electrode active material: Lithium dihydrogen phosphate, ferrous oxalate, polyethylene glycol with a weight average molecular weight of 1000, polyethylene glycol with a weight average molecular weight of 1500, titanium dioxide, vanadium pentoxide, and magnesium oxide were mixed evenly in methanol and ground to obtain a mixed raw material. The ratio of lithium dihydrogen phosphate to ferrous oxalate resulted in a lithium to iron molar ratio of 1.02:1.0. The particle size D of ferrous oxalate was... 10 With a particle size of 6.2 μm and a diameter D 50 With a particle size of 60.8 μm and a diameter D 90 The thickness is 106.5 μm, and the mass content of Fe in ferrous oxalate is 30.6%, while the mass content of ferric iron is 0.03%.

[0328] The mixed raw materials are ball-milled multiple times and demagnetized in a ball mill to obtain a mixed slurry. The number of grinding cycles and time are controlled, and the particle size Dv of the resulting mixed slurry is determined. 50 It is 3.1 μm.

[0329] The spray-dried slurry yields a dried precursor powder, which is light yellow in appearance and uniform in color.

[0330] The precursor powder was placed in a sintering furnace and heated from 25°C to 360°C at a rate of 2°C / min under a nitrogen atmosphere, and held at that temperature for 3.5 h. Then, the temperature was increased to a second temperature of 775°C at a rate of 5°C / min and held at that temperature for 10 h, followed by cooling. Based on the total mass of the positive electrode active material, the mass content of Ti was 1050 ppm, the mass content of V was 950 ppm, and the mass content of Mg was 1500 ppm.

[0331] The obtained material was crushed using an airflow pulverization method with a staged frequency of 22Hz and a pulverizing airflow of 0.55MPa to obtain lithium iron phosphate cathode active material with carbon material on its surface.

[0332] The D10, D50, D90, and Dv50 mentioned above refer to the data obtained by testing using the Malvern laser scattering method.

[0333] (2) Preparation of positive electrode sheet

[0334] The above-mentioned positive electrode active material (93.9% by mass), conductive agent (2% by mass), and binder polyvinylidene fluoride (3% by mass) were mixed in the solvent N-methylpyrrolidone. Then, dispersant HNBR (1.1% by mass) was added, and the mixture was thoroughly mixed, stirred, and dispersed in a stirring tank to form a positive electrode slurry. After the stirring process, the positive electrode slurry was transported to the coating process. The mass percentages of the positive electrode active material, conductive agent, binder, and dispersant were calculated based on the total mass of solids in the positive electrode slurry. The conductive agent included conductive carbon black (1.33% by mass) and single-walled carbon nanotubes (0.67% by mass), and the specific surface area of ​​the conductive carbon black was 85 m². 2 / g, oil absorption value of 200ml / 100g, average length of single-walled carbon nanotubes of 30μm, specific surface area of ​​300m² 2 / g, the mass content of metallic impurities in single-walled carbon nanotubes is <1wt%;

[0335] The positive electrode slurry was transferred and coated onto a current collector aluminum foil, dried, and then hot-pressed to obtain a positive electrode film with a single-sided thickness of 104.87 μm and a compaction density of 2.36 g / cm³. 3 The positive electrode sheet. The stirring includes pre-stirring and main stirring. The stirring speed of pre-stirring is lower than that of main stirring. The revolution speed of pre-stirring is 25 rpm, the rotation speed is 500 rpm, and the pre-stirring time is 15 min.

[0336] The hot pressing process includes three hot rolling processes, with the hot rolling pressure increasing sequentially to 35 tons, 55 tons, and 75 tons. The hot rolling temperature is 65℃. Before the first hot rolling compaction, the electrode sheet is heated to 50℃. The compaction density here refers to the compaction density of the battery cell under full discharge conditions, and its testing method is described above.

[0337] The positive electrode sheets are slit and punched into specified shapes, and then the punched positive electrode sheets are sorted by weight using a weighing and sorting machine for stacking by a stacking machine.

[0338] Example 3

[0339] (1) Preparation of positive electrode active material

[0340] Lithium carbonate, ferric phosphate, sucrose, glucose, titanium dioxide, vanadium pentoxide, and magnesium oxide are added to water and mixed in a premixing tank at 1800 rpm. The ratio of lithium carbonate to ferric phosphate is such that the molar ratio of iron to phosphorus is 0.975, the mass content of glucose is 3.8% of that of ferric phosphate, and the mass content of sucrose is 1.9% of that of ferric phosphate.

[0341] The mixed raw materials were ground twice in a sand mill. The first grinding was performed using 0.6 mm diameter zirconia balls at 500 rpm for 1 hour, with a grinding chamber pressure of less than 0.3 MPa. The second grinding was then performed to obtain a mixed slurry. The particle size D of the mixed slurry was... V50 It is 0.43 μm;

[0342] The mixed slurry is spray-dried to obtain precursor powder.

[0343] The precursor powder is sintered to obtain lithium iron phosphate cathode material. The sintering process includes:

[0344] First sintering: The precursor powder is sintered in a nitrogen atmosphere, heated from 25°C to 765°C at a heating rate of 5°C / min, and held at that temperature for 10 hours. After cooling, the first sintered product is obtained.

[0345] Grinding and mixing: Add 0.5% sucrose, 1% glucose, and 3.0% polyethylene glycol (by weight of the first sintered product) to the first sintered product; divide into two groups and grind (third grinding), wherein the particle size D of the first group is... V50 Grinding was stopped when the particle size reached 1.0 μm (grinding conditions: 550 rpm, grinding time 1 h), yielding the first group of ground products; the particle size D of the second group... V50 Grinding was stopped when the particle size reached 0.40 μm (grinding conditions: 500 rpm, grinding time 4 h), and a second set of grinding products was obtained; the first set of grinding products and the second set of grinding products were mixed at a mass ratio of 72:28 to obtain a mixed intermediate product; the mixed intermediate product was spray-dried.

[0346] Second sintering: The dried mixed intermediate product is sintered in a nitrogen atmosphere, heated from 25°C to 800°C at a heating rate of 5°C / min, and held at that temperature for 10 hours. After cooling, the second sintered product is obtained.

[0347] After sintering, the material is cooled to below 100°C, and the second sintering product is crushed using air jet milling to obtain lithium iron phosphate cathode active material with carbon material on its surface. The air jet milling stage frequency is 25 Hz, and the milling pressure is 0.55 MPa. Based on the total mass of the cathode active material, the mass content of Ti is 1050 ppm, the mass content of V is 950 ppm, and the mass content of Mg is 1500 ppm.

[0348] (2) Preparation of positive electrode sheet

[0349] The above-mentioned positive electrode active material (93.9% by mass), conductive agent (2% by mass), and binder polyvinylidene fluoride (3% by mass) were mixed in the solvent N-methylpyrrolidone. Then, dispersant HNBR (1.1% by mass) was added, and the mixture was thoroughly mixed, stirred, and dispersed in a stirring tank to form a positive electrode slurry. After the stirring process, the positive electrode slurry was transported to the coating process. The mass percentages of the positive electrode active material, conductive agent, binder, and dispersant were calculated based on the total mass of solids in the positive electrode slurry. The conductive agent included conductive carbon black (1.33% by mass) and single-walled carbon nanotubes (0.67% by mass), and the specific surface area of ​​the conductive carbon black was 85 m². 2 / g, oil absorption value of 200ml / 100g, average length of single-walled carbon nanotubes of 30μm, specific surface area of ​​300m² 2 / g, the mass content of metallic impurities in single-walled carbon nanotubes is <1wt%;

[0350] The positive electrode slurry was transferred and coated onto a current collector aluminum foil, dried, and then hot-pressed to obtain a positive electrode film with a single-sided thickness of 105.25 μm and a compaction density of 2.36 g / cm³. 3 The positive electrode sheet is dried at a temperature of 95℃ and a speed of 2.0 m / min. The hot pressing process includes three hot rolling processes, with the hot rolling pressure increasing sequentially to 35 tons, 55 tons, and 75 tons; the hot rolling temperature is 65℃. Before the first hot rolling compaction, the electrode sheet is heated to 50℃. The compaction density here refers to the compaction density of the battery cell under full discharge conditions, and its testing method is described below.

[0351] The positive electrode sheets are slit and punched into specified shapes, and then the punched positive electrode sheets are sorted by weight using a weighing and sorting machine for stacking by a stacking machine.

[0352] Example 4

[0353] The preparation method of Example 4 is basically the same as that of Example 1, except that the sintering process of the positive electrode active material and the hot pressing process of the positive electrode sheet are different. Specifically:

[0354] (1) The precursor powder is subjected to two-stage heating and sintering in a nitrogen atmosphere to obtain the positive electrode active material: the temperature is increased from 25℃ to 440℃ at a heating rate of 2℃ / min (first heating stage) and held for 2.5h; the temperature is increased from 440℃ to 760℃ at a heating rate of 5℃ / min (second heating stage) and held for 11h; and then the airflow pulverization intensity is increased to obtain the lithium iron phosphate positive electrode active material with carbon material on the surface.

[0355] (2) The positive electrode slurry was transferred and coated onto the current collector aluminum foil, dried, and hot-pressed to obtain a positive electrode film with a single-sided thickness of 104.68 μm and a compaction density of 2.36 g / cm³. 3 The positive electrode sheet. The transfer coating speed is 20 m / min.

[0356] The hot pressing process includes three hot roller pressing processes, with the hot roller pressing pressure increasing sequentially to 45 tons, 60 tons, and 80 tons. The hot roller temperature is 60℃. Before the first hot roller compaction, the electrode sheet is heated to 40℃.

[0357] Example 5

[0358] The preparation method of Example 5 is basically the same as that of Example 1, except that the preparation method of the positive electrode sheet is adjusted, as follows:

[0359] The positive electrode slurry from Example 1 was transferred and coated onto a current collector aluminum foil and dried. By adjusting the pressure, rolling speed, roll gap, holding time, number of rolling passes, and controlling the coating density in the hot pressing process, a positive electrode sheet with a single-sided thickness of 71.45 μm was obtained through hot pressing; the compaction density of the positive electrode sheet was 2.36 g / cm³. 3 The compaction density here refers to the compaction density of a single battery cell under full discharge conditions; the testing method is described above. Keeping the number of layers in the stack constant, the thickness of the pouch cell is adaptively adjusted according to the thickness of the positive electrode film.

[0360] Example 6

[0361] The preparation method of Example 6 is basically the same as that of Example 1, except that the preparation method of the positive electrode sheet is adjusted, as follows:

[0362] The positive electrode slurry from Example 1 was transferred and coated onto a current collector aluminum foil and dried. By adjusting the pressure, rolling speed, roll gap, holding time, number of rolling passes, and controlling the coating density in the hot pressing process, a positive electrode sheet with a single-sided thickness of 118.66 μm was obtained through hot pressing; the compaction density of the positive electrode sheet was 2.36 g / cm³. 3 The compaction density here refers to the compaction density of a single battery cell under full discharge conditions; the testing method is described above. Keeping the number of layers in the stack constant, the thickness of the pouch cell is adaptively adjusted according to the thickness of the positive electrode film.

[0363] The preparation methods of Examples 7-13 are basically the same as those of Example 1, except that the preparation methods of components A and B in the thermally conductive structural adhesive are adjusted, as shown in Table 4.

[0364] Comparative Example 1

[0365] The preparation method of Comparative Example 1 is basically the same as that of Example 1, except that the preparation process of the positive electrode active material and the hot pressing process of the positive electrode sheet are slightly different. The specific differences include:

[0366] (1) The carbon sources in the mixed raw materials are sucrose and glucose. The mass of sucrose is 2 wt% of the mass of iron phosphate, and the mass of glucose is 4 wt% of the mass of iron phosphate.

[0367] (2) The heating and sintering processes are different. The precursor powder is sintered at least twice in a nitrogen atmosphere. The first sintering temperature is 765℃ and the holding time is 8 hours to obtain the initial sintered product.

[0368] 1.5 wt% (based on the mass of the initial calcination product) of glucose, 3.0 wt% (based on the mass of the initial calcination product) of polyethylene glycol, titanium dioxide, vanadium pentoxide, and magnesium oxide were added to the initial calcination product. After homogenization, the mixture was divided into two groups for secondary grinding. The grinding parameters for the two groups were different, and the particle size distribution (D) of the particles after the first group of grinding was controlled. V 50 is 2.2μm, and the D of the particles after the second group of grinding is... V 50 represents 0.4 μm. The ground particles from the first and second groups were mixed at a mass ratio of 30:70, spray-dried, and then subjected to a second sintering. The second sintering temperature was 815℃, and the temperature was maintained for 10 hours.

[0369] Based on the total mass of the positive electrode active material, the mass content of Ti is 1050 ppm, the mass content of V is 950 ppm, and the mass content of Mg is 1500 ppm.

[0370] (3) The positive electrode slurry was transferred and coated onto the current collector aluminum foil, dried, and hot-pressed to obtain a positive electrode film with a single-sided thickness of 105.36 μm and a compaction density of 2.36 g / cm³. 3 The positive electrode sheet is dried at a temperature of 95℃ and a speed of 2.0 m / min. The hot pressing process includes three hot rolling processes, with the hot rolling pressure increasing sequentially to 35 tons, 55 tons, and 70 tons; the hot rolling temperature is 65℃. Before the first hot rolling compaction, the electrode sheet is heated to 50℃. The compaction density here refers to the compaction density of the battery cell under full discharge conditions, and its testing method is described above.

[0371] The preparation method of Comparative Example 2 is basically the same as that of Example 1, except that the preparation method of the diaphragm is adjusted, as follows:

[0372] Polyvinylidene fluoride (PVDF) and dispersant are added to deionized water and stirred until homogeneous. Thickener and water-based binder are added to the stirred solution and stirred until homogeneous in a grinding mill to obtain a bonding layer slurry. The bonding layer slurry is sprayed onto a base film with a double-sided ceramic layer and pre-evaporated at 80°C and dried at 90°C to obtain a membrane with an island-like bonding layer.

[0373] The thickness of the base film is 8 μm, the thickness of the single-sided ceramic layer is 3 μm, and the thickness of the single-sided adhesive layer is 1 μm.

[0374] Test method:

[0375] 1. Probability of encapsulation failure of individual pouch cells

[0376] At 25°C, the pouch cell in the battery device is charged to 3.65V at a 2C charging rate, which is equal to the nominal capacity of the individual pouch cells. Then, it is charged at a constant voltage of 3.65V to 0.05C. After charging is completed, the charging circuit of the battery device is disconnected and left to stand for 10 minutes. Then, the pouch cell is discharged to 2.5V at a 2C discharging rate, which is equal to the nominal capacity of the individual pouch cells. After standing for 10 minutes, one charge-discharge cycle is recorded. The cycle is paused when the number of cycles reaches 1300. The individual pouch cells in the battery device are disassembled. When misalignment and peeling occur between the encapsulation layer and the metal layer in the packaging bag near the current lead, it is considered that the pouch cell has experienced encapsulation failure. Ten pouch cells are observed simultaneously in each set of embodiments or comparative examples, and the probability of encapsulation failure is calculated.

[0377] 2. Number of cycles corresponding to 80% capacity decay

[0378] At 25°C, the battery pack cells in the device are charged to 3.65V at a charging rate of 0.5C, which is equivalent to the nominal capacity of the individual cells. Then, they are charged at a constant voltage of 3.65V to 0.05C. After charging is complete, the charging circuit of the battery pack is disconnected and left to stand for 10 minutes. Then, the battery pack cells are discharged to 2.5V at a discharge rate of 1C, which is equivalent to the nominal capacity of the individual cells. After standing for 10 minutes, one charge-discharge cycle is counted as one cycle. The test is stopped when the capacity of the battery pack is reduced to 80% of the nominal capacity. This number of cycles is recorded as the number of cycles corresponding to the 80% capacity reduction.

[0379] 3. Thermal conductivity test of thermally conductive structural adhesive.

[0380] At 25°C, the battery pack cells in the battery device were charged to 3.65V at a 2C charging rate, equal to the nominal capacity of each cell. Then, they were charged at a constant voltage of 3.65V to 0.05C. After charging, the charging circuit was disconnected, and the battery was allowed to stand for 10 minutes. Then, the battery was discharged to 2.5V at a 2C discharging rate, equal to the nominal capacity of each cell, and allowed to stand for 10 minutes. This one charge-discharge cycle constituted one cycle. The cycle count was recorded after 300 cycles, and the highest surface temperature of the cell in each embodiment was recorded using infrared thermal imaging, in °C. As shown in Table 4, using the highest temperature of Example 2 as a benchmark, the percentage of the highest temperatures of Examples 1 and 7-13 compared to the highest temperature of Example 2 was calculated. The lower the percentage, the better the thermal conductivity of the thermally conductive structural adhesive used in that embodiment.

[0381] Test results:

[0382] Table 1

[0383] Table 2

[0384] As can be seen from the comparison of the embodiments and comparative examples, the embodiments of this application integrate and assemble lithium transition metal phosphate soft-pack battery cells into a housing using a module-free integration method. When the area of ​​particles with a diameter greater than or equal to 1 μm in the cross-section of the positive electrode film along the thickness direction of the electrode sheet accounts for 12%-40%, and the adhesive layer of the separator is a continuous layer with a porous structure, and the adhesive layer includes vinylidene fluoride polymer, the soft-pack battery cell not only has a high capacity, but also further improves the safety performance of the soft-pack battery cell.

[0385] Table 3

[0386] As can be seen from the comparison between Example 3 and Examples 1 and 2, in the cross-section of the positive electrode film along the thickness direction of the electrode sheet, the median L of the sphericity in the cumulative distribution curve of the sphericity area of ​​particles with a particle size greater than or equal to 1 μm is... A50 When the value is 0.69-0.75, it is beneficial to improve the cycle performance of the pouch cell while maintaining high capacity.

[0387] As can be seen from the comparison between Examples 1, 5, and 6, the single-sided thickness of the positive electrode film is 90μm-120μm, which is beneficial to further improve the capacity of the soft-pack battery cell.

[0388] Table 4

[0389] As can be seen from the comparison between Example 7 and Examples 1 and 8, when the thermal conductivity of the thermally conductive structural adhesive is 0.8 W / (m·K)-1.2 W / (m·K) at 85°C, it is beneficial to improve the thermal conductivity of the thermally conductive structural adhesive and reduce the temperature rise rate of the battery.

[0390] As can be seen from the comparison between Examples 9-11 and Examples 12 and 13, when the energy storage modulus of the thermally conductive structural adhesive is 300MPa-800MPa at a vibration frequency of 0.1Hz at room temperature, it is beneficial to improve the thermal conductivity of the thermally conductive structural adhesive and reduce the temperature rise rate of the battery.

[0391] It should be noted that this application is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this application are included in the technical scope of this application. Furthermore, various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing by combining some of the constituent elements of the embodiments, without departing from the spirit of this application, are also included in the scope of this application.

Claims

1. A battery device, characterized by, include: The housing includes a support plate and a frame surrounding the outer periphery of the support plate, wherein the support plate is fixedly connected to the frame. Multiple pouch battery cells are stacked and housed within a housing in a first direction; each pouch battery cell has a rated capacity greater than or equal to 50 Ah and less than or equal to 300 Ah; the surface of each pouch battery cell includes a first surface and a second surface, the area of ​​the first surface being greater than the area of ​​the second surface; the first surfaces of the multiple pouch battery cells are arranged opposite each other along the first direction; and the support plate is arranged opposite to the second surfaces of the multiple pouch battery cells along a second direction. The housing is provided with at least one connecting beam extending along a third direction. The connecting beam is fixedly connected to the support plate and / or the frame. At least one soft-pack battery cell abuts against the connecting beam along the first direction. The first direction, the second direction, and the third direction are perpendicular to each other. The soft-pack battery cell includes a packaging bag, an electrode assembly, and a current lead. The electrode assembly is housed inside the packaging bag. One end of the current lead is connected to the electrode assembly, and the other end of the current lead is located outside the packaging bag. The current lead and the packaging bag are encapsulated and connected. The electrode assembly includes a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode. The positive electrode includes a positive current collector and a positive electrode film disposed on at least one side of the positive current collector. The positive electrode film includes a positive active material, and the positive active material includes lithium transition metal phosphate particles with carbon material disposed on at least a portion of their surface. In the cross-section of the positive electrode film layer along the thickness direction of the electrode sheet, the area ratio of particles with a particle size greater than or equal to 1 μm is 12%-40%. The separator includes a base membrane, ceramic layers disposed on both sides of the base membrane, and an adhesive layer disposed on at least the side of the ceramic layers away from the base membrane, the adhesive layer being a continuous layer with a porous structure, and the adhesive layer comprising a vinylidene fluoride polymer.

2. The battery device of claim 1, wherein Each of the aforementioned pouch cell has a rated capacity greater than or equal to 100 Ah and less than or equal to 200 Ah.

3. The battery device according to claim 1 or 2, characterized by In the cross-section of the positive electrode film layer along the thickness direction of the electrode sheet, the area of ​​particles with a diameter of 1μm-5μm accounts for 12%-37%.

4. The battery device according to any one of claims 1 to 3, characterized by, In a section of the positive electrode film layer along the thickness direction of the electrode tab, the median number L of sphericity in the cumulative distribution curve of sphericity of particles with a particle size of 1 μm or more A50 0.6-0.8, optionally 0.67-0.75, further optionally 0.69-0.

75.

5. The battery device according to any one of claims 1 to 4, characterized by, The median value C of graphitization degree in the cumulative distribution curve of graphitization degree C value obtained by the positive electrode film layer in the laser microscopic confocal Raman spectrometer face scanning mode 50 is 1.0-1.2, wherein the graphitization degree C value is I G / I D , wherein I G represents the G peak intensity of Raman spectrum at 1580±100 cm - 1 , I D represents the D peak intensity of Raman spectrum at 1350±100 cm -1 .

6. The battery device according to any one of claims 1 to 5, characterized by, The median value B of the coating value in the cumulative distribution curve of the coating value B obtained by the positive electrode film layer under the laser microscopic confocal Raman spectrometer face scanning mode 50 is 0.3-0.6, wherein the coating value B is I P / I D , wherein I P represents the P peak intensity of the Raman spectrum at 948±100cm -1 , I D represents the D peak intensity of the Raman spectrum at 1350±100cm -1 .

7. The battery device according to any one of claims 1 to 6, characterized by, The lithium-containing transition metal phosphate particles include magnesium. Based on the total mass of the lithium-containing transition metal phosphate particles in the positive electrode film, the mass content of magnesium is 1000ppm-3000ppm, and can be selected as 1000ppm-2000ppm.

8. The battery device according to any one of claims 1 to 7, characterized by, The lithium-containing transition metal phosphate particles include titanium. Based on the total mass of the lithium-containing transition metal phosphate particles in the positive electrode film, the mass content of titanium is 500ppm-8000ppm, and can be selected as 1000ppm-3000ppm.

9. The battery device according to any one of claims 1 to 8, characterized by, The lithium-containing transition metal phosphate particles include vanadium. Based on the total mass of the lithium-containing transition metal phosphate particles in the positive electrode film, the mass content of vanadium is 500ppm-5000ppm, and can be selected as 500ppm-3000ppm.

10. The battery device according to any one of claims 1 to 9, characterized by, The soft package battery monomer in full discharge state, the compaction density of the positive pole piece is 2.3g / cm 3 -2.6g / cm 3 .

11. The battery device according to any one of claims 1 to 10, characterized by, The porosity of the positive electrode film is 14%-22%.

12. The battery device according to any one of claims 1 to 11, characterized by, The positive electrode film layer further includes a conductive agent, which includes carbon nanotubes. The carbon nanotubes include one or more of single-walled carbon nanotubes, few-walled carbon nanotubes, and multi-walled carbon nanotubes. Based on the mass of the positive electrode film layer, the mass content of carbon nanotubes is 0.05%-2.5%.

13. The battery device of claim 12, wherein, The conductive agent also includes conductive carbon black, and the mass content of conductive carbon black is 0.05%-2.5% based on the mass of the positive electrode film.

14. The battery device according to claim 12 or 13, characterized by, Based on the total area of ​​the cross-section of the positive electrode film along the thickness direction of the electrode sheet, the total area ratio of the agglomeration region of the conductive agent is 0.2%-6.0%, and can be selected as 1.5%-5.0%; the agglomeration region of the conductive agent includes carbon nanotubes and conductive carbon black.

15. The battery device according to any one of claims 1 to 14, characterized by, The thickness of the positive electrode film layer on one side is 70μm-120μm, optionally 90μm-120μm, and further optionally 100μm-120μm.

16. The battery device of any one of claims 1 to 15, wherein, The length L0 of the soft-pack battery cell is 500mm-1250mm; the width W0 is 100mm-150mm; and the thickness H0 is 14mm-22mm.

17. The battery device of any one of claims 1 to 16, wherein, The packaging bag includes an encapsulation layer, a metal layer, and a protective layer stacked sequentially from the inside of the battery cell to the outside of the battery cell. The metal layer includes aluminum; the encapsulation layer and the protective layer include resin materials.

18. The battery device of claim 17, wherein, The encapsulation layer includes a polypropylene (PP) layer, and optionally, the encapsulation layer includes a polypropylene (PP) layer and a modified polypropylene (PPa) layer disposed between the polypropylene (PP) layer and the metal layer; the protective layer includes one or more of nylon and polyethylene terephthalate (PET).

19. The battery device of claim 18, wherein, The modified polypropylene (PPa) layer comprises maleic anhydride-grafted polypropylene.

20. The battery device of any one of claims 1-19, wherein, The packaging bag is heat-sealed at 180℃-220℃, with a possible temperature of 200℃-210℃.

21. The battery device of any one of claims 1-20, wherein, A thermal management component is provided between the support plate of the housing and the second surface of the soft-pack battery cell. The thermal management component is used to regulate the temperature of the soft-pack battery cell. A thermally conductive structural adhesive is provided between the thermal management component and the second surface of the soft-pack battery cell.

22. The battery device of any one of claim 21, wherein, At 85°C, the thermal conductivity of the thermally conductive structural adhesive is greater than or equal to 0.4 W / (m·K), which can be selected as 0.4 W / (m·K)-1.2 W / (m·K), and more preferably 0.8 W / (m·K)-1.2 W / (m·K).

23. The battery device of any one of claims 21 or 22, wherein, The thermally conductive structural adhesive has a storage modulus of 260MPa-1000MPa at a vibration frequency of 0.1Hz at room temperature, which can be selected as 300MPa-800MPa, and further selected as 300MPa-600MPa.

24. The battery device of any one of claims 21-23, wherein, The glass transition temperature of the thermally conductive structural adhesive is 50℃-60℃.

25. The battery device of any one of claims 21-24, wherein, The thermally conductive structural adhesive comprises polyurethane resin and thermally conductive filler particles dispersed in the polyurethane resin; the thermally conductive filler particles comprise one or more of aluminum hydroxide particles and boron nitride particles.

26. The battery device of claim 25, wherein, Based on the total mass of the thermally conductive structural adhesive, the mass percentage of the thermally conductive filler particles is 20%-70%, optionally 45%-65%.

27. The battery device of any one of claims 21-26, wherein, The projection of the thermally conductive structural adhesive on the first surface does not overlap with the projection of the negative electrode sheet on the first surface.

28. The battery device of any one of claims 21-27, wherein, At least some of the pouch cell units are provided with double-sided adhesive, and a gap is provided between the double-sided adhesive and the thermally conductive structural adhesive.

29. An electrical device, comprising: The electrical device includes a battery device as described in any one of claims 1 to 28, the battery device being used to provide electrical energy.

30. An energy storage device, comprising: The energy storage device includes a battery device as described in any one of claims 1 to 28, the battery device being used to store electrical energy.