Memory and preparation method therefor

By using 3D stacking technology and lateral etching thin film deposition process, memory is fabricated, which solves the density and process bottlenecks of traditional silicon-based DRAM, realizes the integration of high-density memory cells and low power consumption, and simplifies the manufacturing process.

WO2026237173A1PCT designated stage Publication Date: 2026-11-19INST OF MICROELECTRONICS CHINESE ACAD OF SCI LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2025/110775
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-14
Filing Date
2025-07-26
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Traditional silicon-based DRAM faces challenges such as increased leakage current, shortened data retention time, and complex and costly manufacturing processes during the shrinking process, making it difficult to further increase storage density.

Method used

The memory cell is fabricated using 3D stacking technology and lateral etching thin film deposition process. By alternately growing isolation layer, conductive layer and sacrificial layer on the substrate, through-holes are formed and semiconductor and conductive materials are deposited to achieve three-dimensional stacking of memory cells. IGZO material is used to reduce leakage current.

Benefits of technology

It achieves the integration of high-density memory cells, increases memory capacity, simplifies the process and reduces costs, and reduces the need for frequent refresh operations by reducing leakage current, thereby reducing power consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2025110775_19112026_PF_FP_ABST
    Figure CN2025110775_19112026_PF_FP_ABST
Patent Text Reader

Abstract

A memory and a preparation method therefor. The preparation method comprises the following steps: alternately growing a thin film stack structure sequentially on a surface of a substrate; etching deep holes downward in the direction perpendicular to a film layer, so as to form penetrating first channels (4) and second channels (5); performing lateral etching at positions of the first channels (4) and the second channels (5) to form lateral holes; depositing a gate dielectric layer (8); depositing a semiconductor material layer (9) to fill the lateral holes; etching the semiconductor material layer (9), and retaining part of the semiconductor material layer (9) within the lateral holes; depositing a conductive material (10) to fill the first channels (4) and the lateral holes; laterally etching the conductive material (10), and retaining the conductive material (10) in the first channels (4) and the lateral holes; depositing a gate dielectric layer (8) to cover the conductive material (10); depositing the conductive material (10) to fill the second channels (5); performing chemical mechanical polishing for planarization; and forming isolation trenches (11) and filling the same with an isolation material (12). The present invention realizes the integration of high-density storage units by means of 3D stacking technology, thereby effectively increasing the capacity of a memory and satisfying the requirements for high-density storage applications.
Need to check novelty before this filing date? Find Prior Art

Description

A memory and its fabrication method

[0001] [Amended according to Regulation 26, 09.10.2025] This application claims priority to Chinese Patent Application No. 2025106207526, filed on May 14, 2025, entitled "A Memory and a Method for Manufacturing the Same", the entire contents of which are incorporated herein by reference. Technical Field

[0002] This invention relates to the field of memory technology, and in particular to a memory and its fabrication method. Background Technology

[0003] DRAM (Dynamic Random Access Memory) is a core memory technology in modern computer systems, primarily used for main memory and cache storage. Its high speed, low cost, and high density make it a crucial component for data storage in computer systems. The basic working principle of DRAM is to store each bit of data using memory cells composed of transistors and capacitors. Transistors control the charging and discharging state of the capacitors, thus determining the writing and reading of bits; capacitors store electrical charge, and the presence or absence of charge represents the value of the stored data bits. Silicon-based 1T1C DRAM is currently the most common memory implementation scheme, increasing storage density by continuously shrinking feature sizes. However, with advancements in process technology, traditional silicon-based DRAM is facing a series of physical limits and manufacturing challenges.

[0004] As DRAM cell sizes shrink, leakage current increases in traditional silicon-based 1T1C memory cells, leading to shorter data retention times and requiring more frequent refresh operations. This increases power consumption and reduces efficiency. Further miniaturization of traditional silicon-based 1T1C DRAM features still heavily relies on high-precision photolithography, resulting in complex and costly manufacturing processes, and further increases in storage density are difficult to achieve. In current planar 1T1C designs, increasing storage density requires continuously improving semiconductor manufacturing precision to achieve miniaturized device dimensions. With the decline of Moore's Law in the semiconductor industry, size miniaturization is gradually reaching a bottleneck.

[0005] In view of this, the present invention is proposed. Summary of the Invention

[0006] The purpose of this invention is to provide a memory and its fabrication method. By using 3D stacking technology, high-density memory cells are integrated, effectively improving the memory capacity and meeting the needs of high-density memory applications. This invention can solve the performance bottlenecks and process challenges faced by traditional silicon-based DRAM.

[0007] A first aspect of the present invention provides a method for fabricating a memory, comprising the following steps:

[0008] S1. An isolation layer, a conductive layer, a sacrificial layer, and a conductive layer are sequentially and alternately grown on the substrate surface to obtain a thin film stacked structure;

[0009] S2. Deep holes are etched downwards along a direction perpendicular to the film layer on the thin film stacked structure to form several through-holes and second holes.

[0010] S3. The sacrificial layer is laterally etched at the positions of the first and second channels to form transverse holes;

[0011] S4. Deposit a gate dielectric layer on the upper surface of the first channel, the second channel, the transverse holes and the thin film stack structure;

[0012] S5. Deposit a semiconductor material layer on the surface of the gate dielectric layer to fill the lateral holes;

[0013] S6. Etch the semiconductor material layer while retaining part of the semiconductor material layer inside the lateral hole;

[0014] S7. Deposit conductive material on the surface of the gate dielectric layer to fill the first channel and the lateral holes;

[0015] S8. Etch conductive material while retaining the conductive material in the first channel and the transverse holes;

[0016] S9. Deposit a gate dielectric layer to cover the conductive material;

[0017] S10. Deposit conductive material on the surface of the gate dielectric layer to fill the second channel;

[0018] S11. Perform chemical mechanical polishing to expose the upper surface of the thin film stacked structure;

[0019] S12. Perform deep trench isolation and fill with isolation material.

[0020] Preferably, in step S1, the uppermost layer of the thin film stack structure is an isolation layer.

[0021] Preferably, in step S2, the diameter of the first channel is smaller than the diameter of the second channel.

[0022] Preferably, the diameter of the first channel is 10-120 nm, and a higher precision photolithography machine can be used to achieve small hole etching; while ensuring that the diameter of the first channel is smaller than the diameter of the second channel, the diameter of the second channel is adjusted accordingly based on the diameter of the first channel, preferably 20-220 nm; correspondingly, the distance between the first channel and the second channel is also adjusted adaptively, preferably 30-120 nm.

[0023] Preferably, in step S3, a first transverse hole is formed at the first channel position, and a second transverse hole is formed at the second channel position, wherein the first transverse hole and the second transverse hole are interconnected.

[0024] Preferably, in step S5, the semiconductor material layer is made of metal oxide, more preferably indium gallium zinc oxide (IGZO). Utilizing the wide bandgap characteristics of IGZO material, leakage current of the memory cell can be effectively reduced, thereby increasing data retention time, reducing reliance on frequent refresh operations, and lowering overall power consumption.

[0025] Preferably, in step S5, a semiconductor material layer is deposited on the surface of the gate dielectric layer, and the first and second channels are not filled, maintaining a through-hole structure.

[0026] Preferably, in step S6, the semiconductor material layer is etched, retaining a portion of the semiconductor material in the first lateral hole and the second lateral hole, and the semiconductor material layers between the first lateral hole and the second lateral hole are connected.

[0027] Preferably, in step S7, a conductive material is deposited on the surface of the gate dielectric layer, and the second channel is not filled, maintaining a continuous hollow structure.

[0028] Preferably, in the thin film stacked structure, the thickness of the isolation layer is 15-25 nm, and the material of the isolation layer is Si3N4; the thickness of the conductive layer is 20-40 nm, and the material of the conductive layer is metal or metal oxide, preferably TiN; the thickness of the sacrificial layer is 20-40 nm, and the material of the sacrificial layer is SiO2.

[0029] Preferably, the thickness of the gate dielectric layer is 6-10 nm, and the material of the gate dielectric layer is selected from materials with high dielectric constant, such as HfO2, Al2O3, etc.

[0030] Preferably, the thickness of the semiconductor material layer is 15-20 nm.

[0031] Preferably, the thickness of the conductive material is 10-200 nm, and the conductive material is a metal or metal oxide, such as W / TiN, Mo, ITO, etc.

[0032] Preferably, the insulating material is Al2O3.

[0033] In a second aspect, the present invention provides a memory prepared by the above-described preparation method.

[0034] Specifically, the memory includes a plurality of memory cells, each memory cell including: a transistor and a capacitor, the transistor including: a source drain, a channel and a gate; the gate is located on the upper and lower sides of the channel, and a gate dielectric layer is disposed between the gate and the channel; the source drain is located on the left and right sides of the channel.

[0035] The present invention has at least the following beneficial effects:

[0036] This invention achieves three-dimensional stacking of DRAM memory cells through 3D stacking technology. As the number of stacking layers increases, the storage density of DRAM can be increased significantly, realizing the integration of high-density memory cells, effectively improving the capacity of the memory, and meeting the needs of future high-density storage applications. In addition, the transistor structure is manufactured by lateral etching and thin film deposition technology, which effectively avoids high-precision photolithography, simplifies the process flow, and greatly reduces manufacturing costs. Attached Figure Description

[0037] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.

[0038] Figure 1 is a schematic diagram of the structure after the thin film stacking structure is grown on the substrate in step S1 of the present invention.

[0039] Figure 2 is a partial schematic diagram after the thin film stacking structure is grown on the substrate in step S1 of the present invention;

[0040] Figure 3 is a schematic diagram of the structure after the formation of the first channel and the second channel in step S2 of the present invention.

[0041] Figure 4 is a partial schematic diagram after the formation of the first channel and the second channel in step S2 of the present invention.

[0042] Figure 5 is a schematic diagram of the structure after the transverse hole is formed in step S3 of the present invention;

[0043] Figure 6 is a partial schematic diagram after the transverse hole is formed in step S3 of the present invention;

[0044] Figure 7 is a schematic diagram of the structure after the gate dielectric layer is deposited in step S4 of the present invention;

[0045] Figure 8 is a partial schematic diagram after the deposition of the gate dielectric layer in step S4 of the present invention;

[0046] Figure 9 is a schematic diagram of the structure after the semiconductor material layer is deposited in step S5 of the present invention;

[0047] Figure 10 is a partial schematic diagram after the semiconductor material layer is deposited in step S5 of the present invention;

[0048] Figure 11 is a schematic diagram of the structure after etching the semiconductor material layer in step S6 of the present invention;

[0049] Figure 12 is a partial schematic diagram after etching the semiconductor material layer in step S6 of the present invention;

[0050] Figure 13 is a schematic diagram of the structure after the conductive material is deposited in step S7 of the present invention;

[0051] Figure 14 is a partial schematic diagram after the deposition of conductive material in step S7 of the present invention;

[0052] Figure 15 is a schematic diagram of the structure after etching the conductive material in step S8 of the present invention.

[0053] Figure 16 is a partial schematic diagram after etching the conductive material in step S8 of the present invention.

[0054] Figure 17 is a schematic diagram of the structure after the gate dielectric layer is deposited in step S9 of the present invention;

[0055] Figure 18 is a partial schematic diagram after the deposition of the gate dielectric layer in step S9 of the present invention;

[0056] Figure 19 is a schematic diagram of the structure after the conductive material is deposited in step S10 of the present invention.

[0057] Figure 20 is a partial schematic diagram after the deposition of conductive material in step S10 of the present invention;

[0058] Figure 21 is a schematic diagram of the structure after chemical mechanical polishing in step S11 of the present invention;

[0059] Figure 22 is a partial schematic diagram after chemical mechanical polishing in step S11 of the present invention;

[0060] Figure 23 is a schematic diagram of the structure after deep trench isolation in step S12 of the present invention;

[0061] Figure 24 is a partial schematic diagram after deep trench isolation in step S12 of the present invention;

[0062] Figure 25 is a schematic diagram of the structure after isolating the filling material in step S12 of the present invention;

[0063] Figure 26 is a partial schematic diagram after the isolation of the filling material in step S12 of the present invention.

[0064] Explanation of reference numerals in the attached figures: 1. Isolation layer; 2. Conductive layer; 3. Sacrificial layer; 4. First channel; 5. Second channel; 6. First lateral hole; 7. Second lateral hole; 8. Gate dielectric layer; 9. Semiconductor material layer; 10. Conductive material; 11. Deep trench; 12. Isolation material. Detailed Implementation

[0065] It should be noted that the following detailed descriptions are illustrative and intended to provide further explanation of this application. Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains.

[0066] It should be noted that the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the exemplary embodiments according to this application. As used herein, the singular form includes the plural form unless the context clearly indicates otherwise. Furthermore, it should be understood that when the terms "comprising" and / or "including" are used in this specification, they indicate the presence of features, steps, operations, devices, components, and / or combinations thereof.

[0067] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0068] Example

[0069] This embodiment provides a method for fabricating a memory, including the following steps:

[0070] S1. An isolation layer 1, a conductive layer 2, a sacrificial layer 3 and a conductive layer 2 are sequentially and alternately grown on the surface of a substrate to obtain a thin film stacked structure;

[0071] S2. Deep holes are etched downwards along a direction perpendicular to the film layer on the thin film stacked structure to form several through-holes 4 and 5.

[0072] S3. The sacrificial layer 3 is laterally etched at the positions of the first channel 4 and the second channel 5 to form a transverse hole;

[0073] S4. Deposit a gate dielectric layer 8 on the upper surface of the first channel 4, the second channel 5, the transverse holes and the thin film stacked structure;

[0074] S5. Deposit a semiconductor material layer 9 on the surface of the gate dielectric layer 8 to fill the lateral holes;

[0075] S6. Etch semiconductor material layer 9, retaining part of semiconductor material layer 9 inside the transverse hole;

[0076] S7. Deposit conductive material 10 on the surface of gate dielectric layer 8 to fill the first channel 4 and the transverse hole;

[0077] S8. Etch conductive material 10 while retaining the first channel 4 and the conductive material 10 in the transverse hole;

[0078] S9, Deposit gate dielectric layer 8 to cover conductive material 10;

[0079] S10. Deposit conductive material 10 on the surface of gate dielectric layer 8 to fill the second channel 5;

[0080] S11. Perform chemical mechanical polishing to expose the upper surface of the thin film stacked structure;

[0081] S12. Perform deep trench 11 isolation and fill it with isolation material 12.

[0082] The preparation method of this embodiment will be described in more detail below:

[0083] For step S1, as shown in Figures 1-2, a 20 nm thick isolation layer 1 (Si3N4), a 30 nm thick conductive layer 2 (TiN), a 30 nm thick sacrificial layer 3 (SiO2), and a 30 nm thick conductive layer 2 (TiN) are sequentially and alternately grown on a silicon substrate by chemical vapor deposition (CVD). The top layer of the thin film stack structure is the isolation layer 1, the top layer is the CMP stop layer, and the bottom layer is the etching stop layer, thus obtaining the thin film stack structure.

[0084] For step S2, as shown in Figures 3-4, deep holes are etched downwards along a direction perpendicular to the film layer on the thin film stack structure to form several through first channels 4 with a diameter of 100 nm and second channels 5 with a diameter of 200 nm. The distance between the first channels 4 and the second channels 5 is 100 nm.

[0085] For step S3, as shown in Figures 5-6, the sacrificial layer 3 is laterally etched at the positions of the first channel 4 and the second channel 5, forming a first transverse hole 6 at the position of the first channel 4 and a second transverse hole 7 at the position of the second channel 5. The first transverse hole 6 and the second transverse hole 7 are interconnected.

[0086] For step S4, as shown in Figures 7-8, an 8 nm thick gate dielectric layer 8 (HfO2) is deposited on the upper surface of the first channel 4, the second channel 5, the lateral holes and the thin film stack structure using atomic layer deposition (ALD) process.

[0087] For step S5, as shown in Figures 9-10, an atomic layer deposition process is used to deposit a 16nm thick semiconductor material layer 9 (IGZO) on the surface of the gate dielectric layer 8 to fill the lateral holes.

[0088] For step S6, as shown in Figures 11-12, the semiconductor material layer 9 is wet-etched, retaining a portion of the semiconductor material of the first lateral hole 6 and the second lateral hole 7, and the semiconductor material layer 9 between the first lateral hole 6 and the second lateral hole 7 is connected to form a channel. Above the channel are the gate dielectric layer 8 and the gate, and below the channel are the gate dielectric layer 8 and the gate.

[0089] For step S7, as shown in Figures 13-14, an atomic layer deposition process is used to deposit a 60 nm thick conductive material 10 (W / TiN) on the surface of the gate dielectric layer 8 to fill the first channel 4 and the transverse pores. Growth can be stopped after the first channel 4 is filled. At this time, the second channel 5 is not filled, maintaining the through hollow structure.

[0090] For step S8, as shown in Figures 15-16, the conductive material 10 is wet-etched, retaining the first channel 4 and the conductive material 10 in the lateral hole to form the source and drain, thereby obtaining the transistor structure.

[0091] For step S9, as shown in Figures 17-18, an 8nm thick gate dielectric layer 8 is deposited using an atomic layer deposition process to cover the conductive material 10.

[0092] For step S10, as shown in Figures 19-20, an atomic layer deposition process is used to deposit a 60 nm thick conductive material 10 on the surface of the gate dielectric layer 8 to fill the second channel 5 and form a capacitor.

[0093] For step S11, as shown in Figures 21-22, chemical mechanical polishing (CMP) is performed to smooth the surface and expose the uppermost isolation layer 1 of the thin film stacked structure.

[0094] For step S12, as shown in Figures 23-24, deep trench 11 is isolated, and as shown in Figures 25-26, isolation material 12 (Al2O3) is filled to form a memory with multiple memory cells.

[0095] This embodiment also provides a memory, which is prepared using the method described in this embodiment.

[0096] In this embodiment, the memory includes several memory cells, each memory cell including: a transistor and a capacitor. The transistor includes: a source drain, a channel and a gate; the gate is located on the upper and lower sides of the channel, and a gate dielectric layer 8 is disposed between the gate and the channel. The source drain is located on the left and right sides of the channel.

[0097] In summary, this invention achieves three-dimensional stacking of DRAM memory cells through 3D stacking technology. As the number of stacking layers increases, the storage density of DRAM can be significantly increased, realizing the integration of high-density memory cells, effectively improving memory capacity, and meeting the needs of future high-density storage applications. Moreover, by manufacturing transistor structures through lateral etching and thin-film deposition technologies, high-precision photolithography is effectively avoided, simplifying the process flow and greatly reducing manufacturing costs. In addition, by utilizing the wide bandgap characteristics of IGZO material, the leakage current of memory cells is effectively reduced, thereby improving data retention time, reducing reliance on frequent refresh operations, and lowering overall power consumption.

[0098] The above description does not provide detailed explanations of the technical aspects of each layer's patterning, etching, etc. However, those skilled in the art should understand that various technical means can be used to form layers and regions of the desired shape. Furthermore, to form the same structure, those skilled in the art can also design methods that are not entirely identical to those described above. Additionally, although various embodiments have been described above, this does not mean that the measures in the various embodiments cannot be used advantageously in combination.

[0099] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for producing a memory, characterized by, Includes the following steps: S1. An isolation layer, a conductive layer, a sacrificial layer, and a conductive layer are sequentially and alternately grown on the substrate surface to obtain a thin film stacked structure; S2. Deep holes are etched downwards along a direction perpendicular to the film layer on the thin film stacked structure to form several through-holes and second holes. S3. The sacrificial layer is laterally etched at the positions of the first and second channels to form transverse holes; S4. Deposit a gate dielectric layer on the upper surface of the first channel, the second channel, the transverse holes and the thin film stack structure; S5. Deposit a semiconductor material layer on the surface of the gate dielectric layer to fill the lateral holes; S6. Etch the semiconductor material layer while retaining part of the semiconductor material layer inside the lateral hole; S7. Deposit conductive material on the surface of the gate dielectric layer to fill the first channel and the lateral holes; S8. Etch conductive material while retaining the conductive material in the first channel and the transverse holes; S9. Deposit a gate dielectric layer to cover the conductive material; S10. Deposit conductive material on the surface of the gate dielectric layer to fill the second channel; S11. Perform chemical mechanical polishing to expose the upper surface of the thin film stacked structure; S12. Perform deep trench isolation and fill with isolation material.

2. The production method according to claim 1, characterized by, In step S1, the top layer of the thin film stacked structure is an isolation layer.

3. The preparation method according to claim 1, characterized in that, In step S2, the diameter of the first channel is smaller than the diameter of the second channel.

4. The production method according to claim 3, characterized by, The diameter of the first channel is 80-120 nm, the diameter of the second channel is 180-220 nm, and the distance between the first channel and the second channel is 80-120 nm.

5. The preparation method according to claim 1, characterized in that, In step S3, a first transverse hole is formed at the first channel position, and a second transverse hole is formed at the second channel position. The first transverse hole and the second transverse hole are interconnected.

6. The method of claim 1, wherein, In step S5, the semiconductor material layer is made of metal oxide.

7. The preparation method according to claim 1, characterized in that, In step S5, a semiconductor material layer is deposited on the surface of the gate dielectric layer, and the first and second channels are not filled, maintaining a through-hole structure.

8. The preparation method according to claim 5, characterized in that, In step S6, the semiconductor material layer is etched, retaining a portion of the semiconductor material in the first lateral hole and the second lateral hole, and the semiconductor material layers between the first lateral hole and the second lateral hole are connected.

9. The method of claim 1, wherein, In step S7, conductive material is deposited on the surface of the gate dielectric layer, and the second channel is not filled, maintaining a continuous hollow structure.

10. A memory, comprising: It is prepared by the preparation method according to any one of claims 1-9.