Solar cell, preparation method therefor, and photovoltaic module

By designing an arched protrusion structure on the back of the solar cell to increase the surface area of ​​the interlayer, and utilizing the reflected light from the ground for secondary utilization, the problem of low photon utilization in the interlayer area on the back of the BC solar cell is solved, thereby improving the light absorption and efficiency of the solar cell.

WO2026237182A1PCT designated stage Publication Date: 2026-11-19GCL SYST INTEGRATION TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2025/111024
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-14
Filing Date
2025-07-28
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

The photon utilization rate of the back spacer region of BC solar cells is low, resulting in insufficient utilization of sunlight and significant room for efficiency improvement.

Method used

An arched protrusion structure is designed on the back of the solar cell to increase the surface area of ​​the interlayer. The light reflected from the ground is reused, and the arched protrusion structure is formed by laser processing and wet texturing.

Benefits of technology

This improves the light absorption capacity and light utilization rate of solar cells, thereby increasing their efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2025111024_19112026_PF_FP_ABST
    Figure CN2025111024_19112026_PF_FP_ABST
Patent Text Reader

Abstract

The present application discloses a solar cell, a preparation method therefor, and a photovoltaic module. The solar cell comprises a substrate, wherein the substrate comprises a front surface and a back surface that are disposed opposite to each other, the back surface is divided into a first region, a second region, and a gap region, a first functional structure is disposed in the first region, the first functional structure comprises a p-type doped layer, a second functional structure is disposed in the second region, the second functional structure comprises an n-type doped layer, and the gap region is configured for spacing the first functional structure from the second functional structure; and in a direction from the front surface toward the back surface, the substrate in the gap region is an arch-shaped protrusion structure.
Need to check novelty before this filing date? Find Prior Art

Description

Solar cells, their fabrication methods, and photovoltaic modules

[0001] Cross-reference to related applications

[0002] This application claims priority to Chinese patent application No. 202510621900.6, filed on May 14, 2025, the entirety of which is incorporated herein by reference. Technical Field

[0003] This application relates to the field of solar cell technology, specifically to solar cells, methods for their fabrication, and photovoltaic modules. Background Technology

[0004] In BC (back-contact) solar cells, both the positive and negative electrodes are printed on the back side of the cell, leaving the front side unobstructed. Compared to conventional solar cells, the Jsc (short-circuit current) can be increased by approximately 7%. Currently, BC solar cells rely on the front side to utilize incident photons, resulting in lower utilization of the back gap area. Therefore, the utilization rate of sunlight by BC solar cells needs improvement, and there is significant room for efficiency enhancement. Summary of the Invention

[0005] This application aims to at least partially alleviate or resolve at least one of the aforementioned problems.

[0006] In one aspect of this application, a solar cell is proposed. In some embodiments of this application, the solar cell includes a substrate, the substrate including a front side and a back side disposed opposite to each other, the back side being divided into a first region, a second region, and a spacer region. A first functional structure is disposed on the first region, the first functional structure including a p-type doped layer, and a second functional structure is disposed on the second region, the second functional structure including an n-type doped layer. The spacer region is used to separate the first functional structure and the second functional structure. Along the direction from the front side to the back side, the substrate of the spacer region has an arched protrusion structure. The arched protrusion structure can increase the surface area of ​​the back side spacer region, improving the light absorption capacity of the spacer region; the arched protrusion structure can also reuse light rays that pass through the gaps in the solar cell and are scattered by the ground after reflection by the ground, thereby improving the utilization rate of light by the solar cell and thus improving the efficiency of the solar cell.

[0007] In some embodiments of this application, the height difference between the highest and lowest points of the arched protrusion structure is 1.5 μm to 7 μm. Therefore, the arched protrusion structure can significantly increase the surface area of ​​the back-side spacer region, thereby further improving the light absorption capacity and light utilization rate of the solar cell.

[0008] In some embodiments of this application, the height difference between the surface of the p-type doped layer away from the substrate and the highest point of the arched protrusion structure is ≥3 μm. Therefore, the spacer region can effectively isolate the first functional structure and the second functional structure, thereby contributing to further improvements in the performance of the solar cell.

[0009] In some embodiments of this application, the height difference between the surface of the n-type doped layer away from the substrate and the highest point of the arched protrusion structure is ≥1.5 μm. Therefore, the spacer region can effectively isolate the first and second functional structures, thereby contributing to further improvements in the performance of the solar cell.

[0010] In another aspect of this application, a method for fabricating a solar cell is proposed. In some embodiments of this application, the method for fabricating a solar cell includes: providing a substrate comprising a front side and a back side disposed opposite to each other; dividing the back side into a first region, a second region, and a spacer region; forming a p-type doped layer and a borosilicate glass layer on the back side; removing the borosilicate glass layer and the p-type doped layer from the second region and the spacer region; forming an n-type doped layer and a phosphosilicate glass layer on the back side; performing laser processing on the structures in the first region and the spacer region, wherein the laser energy applied to the spacer region gradually decreases and then gradually increases along the width direction of the spacer region; performing wet texturing to remove the phosphosilicate glass layer, the n-type doped layer, and a portion of the substrate from the spacer region, thereby forming an arched protrusion structure in the substrate of the spacer region. Thus, the laser processing can create varying degrees of looseness in the structure of the spacer region, and the subsequent wet texturing process can form an arched protrusion structure. The back side of the solar cell fabricated using the above method has a high light utilization rate, which is beneficial for improving the efficiency of the solar cell.

[0011] In some embodiments of this application, laser processing is performed on different positions of the interval along the width direction of the interval. Each laser beam strikes the same number of times, and the laser power gradually decreases and then gradually increases. The overlap rate between any two laser beams is ≤5%. Thus, by adjusting the laser power, the structural looseness of the interval can be varied, and after subsequent texturing, an arched protruding structure is formed.

[0012] In some embodiments of this application, a laser beam is used to laser process different positions of the interval along the width direction of the interval. Each laser beam has the same power, and the number of laser strikes gradually decreases and then gradually increases. The overlap rate between the spots of any two laser beams is ≤5%. Thus, by adjusting the number of laser strikes, the structural looseness of the interval can be made to be different, thereby obtaining an arched protruding structure after subsequent texturing.

[0013] In some embodiments of this application, along the width direction of the interval region, the number of laser strikes first gradually decreases by 'a' times and then gradually increases by 'a' times, where 'a' is 1 to 5. This facilitates the formation of a smoother, arched protrusion structure, thereby further increasing the surface area of ​​the interval region and improving the light absorption capacity of the back side.

[0014] In some embodiments of this application, the method for fabricating solar cells satisfies at least one of the following conditions: the energy of each laser beam applied to the spacer region is ≤50μJ; the etching solution used in wet texturing includes sodium hydroxide and / or potassium hydroxide; the arched protrusion structure has multiple pyramid structures, the size of the pyramid structures is 1.5μm to 1.8μm, and the height of the pyramid structures is 0.6μm to 1.2μm.

[0015] In another aspect, this application proposes a photovoltaic module. In some embodiments of this application, the photovoltaic module includes the solar cell described above, or the photovoltaic module includes a solar cell prepared using the methods described above. Thus, the photovoltaic module possesses all the features and advantages of the solar cell described above, which will not be repeated here. In general, the photovoltaic module has high light utilization and efficiency. Attached Figure Description

[0016] The above and / or additional aspects and advantages of this application will become apparent and readily understood from the description of the embodiments taken in conjunction with the following drawings, in which:

[0017] Figure 1 shows a schematic diagram of the structure of a solar cell according to an embodiment of this application;

[0018] Figure 2 shows a partial structural schematic diagram of a solar cell according to an embodiment of this application;

[0019] Figure 3 shows a partial structural schematic diagram of a solar cell according to an embodiment of this application;

[0020] Figure 4 shows a partial structural schematic diagram of a solar cell according to an embodiment of this application;

[0021] Figure 5 shows a partial structural schematic diagram of a solar cell according to an embodiment of this application;

[0022] Figure 6 shows a partial structural schematic diagram of a solar cell according to an embodiment of this application.

[0023] Explanation of reference numerals in the attached figures: 10: Substrate; 11: Front side; 12: Back side; A: First region; B: Second region; C: Spacer region; 20: First functional structure; 21: First tunneling oxide layer; 22: p-type doped layer; 30: Second functional structure; 31: Second tunneling oxide layer; 32: n-type doped layer; 41: Back passivation film; 42: Back antireflection film; 51: Pyramid structure. Detailed Implementation

[0024] The embodiments of this application are described in detail below. Examples of these embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals denote the same or similar elements or elements having the same or similar functions throughout. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain this application, and should not be construed as limiting this application.

[0025] In one aspect of this application, a solar cell is proposed. In some embodiments of this application, referring to FIG1, the solar cell includes a substrate 10, the substrate 10 including a front side 11 and a back side 12 disposed opposite to each other, the back side 12 being divided into a first region A, a second region B and a spacer region C, a first functional structure 20 being disposed on the first region A, the first functional structure 20 including a p-type doped layer 22, a second functional structure 30 being disposed on the second region B, the second functional structure 30 including an n-type doped layer 32, and the spacer region C being used to separate the first functional structure 20 and the second functional structure 30; along the direction from the front side 11 to the back side 12, the substrate of the spacer region C has an arched protrusion structure.

[0026] The arched protrusion design can increase the surface area of ​​the back surface and improve the light absorption capacity of the solar cell. This arched protrusion structure can fully utilize the light that shines on the ground through the gaps in the solar cell and the light scattered by the ground after being reflected by the ground, which is beneficial to improving the efficiency and / or power of the solar cell.

[0027] In some embodiments of this application, the substrate 10 can be an n-type single-crystal silicon wafer. In other embodiments of this application, the substrate 10 can be a p-type single-crystal silicon wafer. The specific thickness of the substrate 10 is not particularly limited in this application, and those skilled in the art can select and set it according to actual needs.

[0028] In some embodiments of this application, the minority carrier lifetime of substrate 10 is >1 ms and the resistivity is 0.5 Ω·cm to 2.1 Ω·cm.

[0029] In some embodiments, the p-type doped layer can be a boron-doped polycrystalline silicon layer, and the n-type doped layer can be a phosphorus-doped polycrystalline silicon layer.

[0030] In some embodiments of this application, the solar cell may be an IBC solar cell or a TBC solar cell.

[0031] In some embodiments of this application, referring to Figures 2 and 3, the height difference h1 between the highest point P1 and the lowest point P2 of the arched protrusion structure can be 1.5 μm to 7 μm. For example, the height difference h1 between the highest point P1 and the lowest point P2 of the arched protrusion structure can be 1.5 μm, 1.8 μm, 2 μm, 2.5 μm, 3 μm, 4 μm, 5 μm, 6 μm, or 7 μm. It should be noted that, referring to Figure 3, the arched protrusion structure has a pyramidal textured surface. The highest point P1 of the arched protrusion structure refers to the apex of the pyramidal structure on the pyramidal textured surface that is furthest from the front surface 11 of the substrate 10, and the lowest point P2 of the arched protrusion structure refers to the apex of the pyramidal structure on the pyramidal textured surface that is furthest from the front surface 11 of the substrate 10. A height difference between the highest and lowest points of the arched protrusion structure within the above range can significantly increase the textured surface area of ​​the interlayer, thereby further improving the light absorption capacity of the solar cell and thus improving the light utilization rate of the solar cell.

[0032] In some embodiments of this application, referring to FIG4, the height difference h3 between the surface of the p-type doped layer 22 away from the substrate 10 and the highest point of the arched protrusion structure can be ≥3μm. For example, the height difference h3 between the surface of the p-type doped layer 22 away from the substrate 10 and the highest point of the arched protrusion structure can be 3μm, 4μm, 5μm, 6μm, 7μm, or 8μm. Therefore, the arched protrusion structure and the p-type doped layer in the first functional structure have a certain height difference, and the arched protrusion structure can play a good isolation role.

[0033] In some embodiments, the height difference h3 between the surface of the p-type doped layer 22 away from the substrate 10 and the highest point of the arched protrusion structure can be 3 μm to 8 μm.

[0034] In some embodiments of this application, referring to Figures 1 and 4, the first functional structure 20 further includes a first tunneling oxide layer 21, and a p-type doped layer 22 is located on the side of the first tunneling oxide layer 21 away from the substrate 10.

[0035] In some embodiments, the first tunneling oxide layer 21 may be a silicon oxide layer.

[0036] In some embodiments, the thickness of the first tunneling oxide layer 21 can be 1.5 nm to 2.5 nm.

[0037] In some embodiments, referring to Figures 1 and 4, the first functional structure 20 may further include a back passivation film 41, which is located on the side of the p-type doped layer 22 away from the substrate 10. In some specific embodiments, the back passivation film 41 may be an alumina passivation film. This passivates the back surface defect structure, reduces carrier recombination, and improves the photoelectric conversion efficiency of the solar cell.

[0038] In some embodiments of this application, referring to Figures 1 and 4, the first functional structure 20 may further include a back antireflection film 42, which is located on the side of the p-type doped layer 22 away from the substrate 10. In some specific embodiments, the back antireflection film 42 may be a silicon nitride antireflection film. This reduces the reflection of incident light, which is beneficial for further improving the light utilization efficiency of the solar cell.

[0039] In some embodiments, referring to FIG1 and FIG4, the first functional structure may include a first tunneling oxide layer 21, a p-type doped layer 22, a back passivation film 41 and a back antireflection film 42, wherein the back passivation film 41 is located on the side of the p-type doped layer 22 away from the substrate 10, and the back antireflection film 42 is located on the side of the back passivation film 41 away from the substrate 10.

[0040] In some embodiments of this application, the first functional structure may further include a first gate line that contacts the p-type doped layer.

[0041] In some embodiments, referring to FIG4, the height difference h2 between the surface of the n-type doped layer 32 away from the substrate 10 and the highest point of the arched protrusion structure can be ≥1.5μm. For example, the height difference h2 between the surface of the n-type doped layer 32 away from the substrate 10 and the highest point of the arched protrusion structure can be 1.5μm, 1.8μm, 2μm, 2.2μm, 2.5μm, 2.7μm, 3μm, or 3.5μm. In some embodiments, the height difference h2 between the surface of the n-type doped layer 32 away from the substrate 10 and the highest point of the arched protrusion structure can be 1.5μm to 3.5μm.

[0042] In some embodiments of this application, referring to Figures 1 and 4, the second functional structure 30 may further include a second tunneling oxide layer 31, with an n-type doped layer 32 located on the side of the second tunneling oxide layer 31 away from the substrate 10.

[0043] In some embodiments of this application, the second tunneling oxide layer 31 may be a silicon oxide layer.

[0044] In some embodiments of this application, the thickness of the second tunneling oxide layer 31 can be 1.5 nm to 2.5 nm.

[0045] In some embodiments of this application, referring to Figures 1 and 4, the second functional structure 30 may further include a back passivation film 41, which is located on the side of the n-type doped layer 32 away from the substrate 10.

[0046] In some embodiments of this application, referring to Figures 1 and 4, the second functional structure 30 may further include a back antireflection film 42, which is located on the side of the n-type doped layer 32 away from the substrate 10.

[0047] In some embodiments of this application, referring to Figures 1 and 4, the second functional structure 30 may include a second tunneling oxide layer 31, an n-type doped layer 32, a back passivation film 41, and a back antireflection film 42 disposed sequentially along the direction from the front side 11 to the back side 12.

[0048] In some embodiments of this application, the second functional structure 30 may further include a second gate line that contacts the n-type doped layer 32.

[0049] In some embodiments of this application, referring to FIG5, the arched protrusion structure has multiple pyramid structures 51. The size of the pyramid structure 51 can be 1.5μm to 1.8μm, and the height of the pyramid structure 51 can be 0.6μm to 1.2μm. The size of the pyramid structure 51 refers to the maximum size of the base of the pyramid structure, and the height of the pyramid structure 51 refers to the distance between the apex and the base of the pyramid structure. In some embodiments, the base of the pyramid structure is a square or approximately square, and the maximum size of the base can be the length of the diagonal of the square.

[0050] In some embodiments of this application, referring to FIG5, a back passivation film 41 and a back antireflection film 42 may be disposed on the spacer region. The back passivation film 41 is located between the substrate and the back antireflection film 42, and the back passivation film 41 and the back antireflection film 42 on the spacer region also have a textured surface structure.

[0051] In some embodiments of this application, referring to FIG6, the width W1 of the first region A can be 300μm to 500μm. For example, the width W1 of the first region A can be 300μm, 350μm, 400μm, 450μm or 500μm.

[0052] In some embodiments of this application, referring to FIG6, the width W3 of the second region B can be 200μm to 400μm. For example, the width W3 of the second region B can be 200μm, 250μm, 300μm, 350μm or 400μm.

[0053] In some embodiments of this application, referring to FIG6, the width W2 of the interval region C can be 50μm to 100μm. For example, the width W2 of the interval region C can be 50μm, 60μm, 70μm, 80μm, 90μm or 100μm.

[0054] The width of the spacer region is approximately 50μm to 100μm, the width of the second region is approximately 200μm to 400μm, and the width of the first region is approximately 300μm to 500μm. The spacer region accounts for approximately 6% of the total area. By setting the substrate of the spacer region as an arched protrusion structure, the textured surface area of ​​the spacer region can be significantly increased, thereby making full use of the back side of the substrate, improving the utilization rate of incident light by the solar cell, and thus helping to improve the efficiency of the solar cell.

[0055] In another aspect of this application, a method for fabricating a solar cell is proposed. In some embodiments of this application, the method for fabricating a solar cell may include the following steps:

[0056] S10: Provides a substrate.

[0057] In some embodiments of this application, the substrate may be an n-type single-crystal silicon wafer or a p-type single-crystal silicon wafer.

[0058] In some embodiments of this application, the substrate includes a front side and a back side disposed opposite to each other, and the back side is divided into a first region, a second region, and a spacer region. The first region is used to provide a first functional structure having a p-type doped layer, the second region is used to provide a second functional structure having an n-type doped layer, and the spacer region is used to separate the first functional structure and the second functional structure.

[0059] Before preparing the tunneling oxide layer, the substrate can be cleaned and polished. In some embodiments, the substrate is cleaned and polished to remove slicing damage and surface contaminants from the n-type / p-type single crystal silicon substrate (101) to form a tower base with a size of 10 μm to 25 μm. The minority carrier lifetime of the n-type / p-type single crystal silicon substrate is >1 ms, and the resistivity is 0.5 Ω·cm to 2.1 Ω·cm.

[0060] S20: A p-type doped layer and a borosilicate glass layer are formed on the back side.

[0061] In some embodiments of this application, S20 may include the following steps:

[0062] S21: A first tunneling oxide layer and an intrinsic polycrystalline silicon layer are formed on the back side.

[0063] In some embodiments of this application, a first tunneling oxide layer can be grown on the 101 surface of the substrate using LPCVD (low-pressure chemical vapor deposition). The growth temperature can be 550°C to 650°C, the growth time can be 5 min to 20 min, and the thickness of the first tunneling oxide layer can be 1.5 nm to 2.5 nm.

[0064] In some embodiments of this application, an intrinsic polysilicon layer can be grown on the side of the first tunneling oxide layer away from the substrate using LPCVD (low-pressure chemical vapor deposition). The growth temperature can be 550°C to 650°C, the growth time can be 3 min to 15 min, and the thickness of the intrinsic polysilicon layer can be 150 nm to 400 nm.

[0065] In some other embodiments of this application, the intrinsic polysilicon layer may be grown directly on the back side of the substrate using LPCVD without forming a first tunneling oxide layer.

[0066] S22: Forms a p-type doped layer and a borosilicate glass layer.

[0067] In some embodiments of this application, boron can be doped into the intrinsic polycrystalline silicon layer by high-temperature diffusion to form a p-type doped layer. The diffusion temperature can be 800°C to 900°C and the diffusion time can be 6 min to 12 min.

[0068] In some embodiments of this application, after forming the p-type doped layer, a borosilicate glass layer (boron oxide layer, BSG) is formed on the p-type doped layer by post-oxidation. The temperature can be 920°C to 980°C, the time can be 25 min to 40 min, and the thickness of the borosilicate glass layer can be 50 nm to 100 nm. The BSG is subsequently used as a mask to prepare for the next laser process.

[0069] S30: Remove the borosilicate glass layer and p-type doped layer in the second region and the spacer region.

[0070] In some embodiments of this application, S30 may include the following steps:

[0071] S31: Laser grooving.

[0072] In some embodiments, lasers can be used to pattern the second region and the interval region to remove the BSG in the second region and the interval region.

[0073] In some embodiments of this application, a laser with an energy of 60 μJ to 100 μJ and a wavelength of 532 nm can be used to pattern grooves on the BSG layer on the back side of the substrate. In some embodiments, the groove width can be 300 μm to 500 μm.

[0074] S32: Removes BSG from the front side of the substrate using a high-concentration HF acid solution from a chain machine. The concentration of the HF acid solution is in the range of 25% to 60%, the length of the acid tank is 4m, and the running speed is 2.0m / min to 3.0m / min.

[0075] S33: Wet etching removes the borosilicate glass layer, p-type doped layer, and a small amount of substrate (removing 2μm to 10μm thick substrate) remaining in the laser-grooved area on the back side, forming a tower base with a size of 20μm to 35μm.

[0076] The borosilicate glass layer and p-type doped layer in the second region and the spacer region can be removed by steps S31-S33, while the borosilicate glass layer and p-type doped layer in the first region are retained.

[0077] When the first tunneling oxide layer is formed on the back side, the wet etching step removes the borosilicate glass layer, p-type doped layer, first tunneling oxide layer, and a small amount of substrate (removing a substrate thickness of 2μm to 10μm) remaining in the laser-grooved area on the back side, as well as the first tunneling oxide layer and a small amount of substrate on the front side, forming a tower base with a size of 20μm-35μm. Steps S31-S33 remove the borosilicate glass layer, p-type doped layer, and first tunneling oxide layer in the second region and the spacer region, while retaining the borosilicate glass layer, p-type doped layer, and first tunneling oxide layer in the first region.

[0078] S40: An n-type doped layer and a phosphorus silicate glass layer are formed on the back side.

[0079] In some embodiments of this application, S40 may include the following steps:

[0080] S41: An intrinsic polycrystalline silicon layer is formed on the back side.

[0081] In some embodiments of this application, a second tunneling oxide layer can be grown on the back side using LPCVD. The growth temperature can be 550℃~650℃, the growth time can be 5min~20min, and the thickness of the second tunneling oxide layer can be 1.5nm-2.5nm.

[0082] In some embodiments of this application, an intrinsic polysilicon layer can be grown on the side of the second tunneling oxide layer away from the substrate using LPCVD. The growth temperature can be 550°C to 650°C, the growth time can be 3 min to 15 min, and the thickness of the intrinsic polysilicon layer can be 150 nm to 400 nm.

[0083] In some other embodiments of this application, an intrinsic polycrystalline silicon layer may be grown directly on one side of the substrate using LPCVD without forming a second tunneling oxide layer.

[0084] S42: Forms an n-type doped layer and a phosphorus glass layer.

[0085] In some embodiments of this application, phosphorus can be doped into the intrinsic polycrystalline silicon layer by high-temperature diffusion to form an n-type doped layer. The diffusion temperature can be 800°C to 900°C and the diffusion time can be 20 min to 30 min.

[0086] In some embodiments of this application, after forming an n-type doped layer, a phosphorus silicate glass layer (containing a phosphorus oxide layer, PSG) is formed on the n-type doped layer by post-oxidation. The temperature can be 900℃~950℃, the time can be 20min~40min, and the thickness of the phosphorus silicate glass layer can be 30nm~60nm. The PSG is subsequently used as a mask to prepare for the next laser process.

[0087] S50: Laser processing is performed on the structures in the first region and the interval region, wherein the laser energy applied to the interval region gradually decreases and then gradually increases along the width direction of the interval region.

[0088] Along the width of the spacer region, the laser energy applied to the spacer region gradually decreases and then gradually increases. This causes the structure of the spacer region to gradually decrease and then gradually increase in looseness along the width direction. In the subsequent wet texturing process, the structure with a smaller looseness reacts more slowly with the etching solution and is etched to a smaller depth, while the structure with a larger looseness reacts more quickly with the etching solution and is etched to a greater depth. This results in an arched protrusion structure with a thickness that gradually increases and then gradually decreases.

[0089] In some embodiments of this application, in the first region, a patterned groove can be made on the BSG layer on the back side of the substrate using a laser with an energy of 60μJ to 100μJ and a wavelength of 532nm. The groove width can be 300μm to 500μm.

[0090] In this application, the laser energy applied to the spacer region can be gradually decreased and then gradually increased along the width direction of the spacer region in different ways.

[0091] In some embodiments of this application, during the laser processing of the spacer region's structure, laser processing is performed on different locations within the spacer region along its width. Each laser beam strikes the spacer region the same number of times, with the laser power gradually decreasing and then increasing. The overlap rate between any two laser beams is ≤5%. Different laser powers result in different energy levels, leading to varying degrees of structural looseness in different regions after processing; higher power corresponds to higher energy, resulting in a looser structure. A laser beam overlap rate of ≤5% allows for better control of the final spacer region's morphology, yielding a smoother, arched protrusion structure. In some embodiments, the overlap rate between any two laser beams can be 0% to 5%, for example, 0%, 0.5%, 0.8%, 1%, 1.2%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, or 5%.

[0092] In some specific embodiments, lasers are used to process different positions in the interval along the width direction of the interval. Each laser beam strikes the same number of times. The energy of the laser is gradually reduced from 50 μJ with a gradient difference of 2 μJ and then gradually increased to 50 μJ with a gradient difference of 2 μJ. The overlap rate between the light spots of any two laser beams is ≤5%.

[0093] In other embodiments of this application, during the laser processing of the spacer region's structure, laser beams are used to process different positions within the spacer region along its width. Each laser beam has the same power (same energy), and the number of laser strikes gradually decreases and then gradually increases. The overlap rate between any two laser beams is ≤5%. With the same laser power but different number of strikes, the degree of structural looseness varies in different regions after processing; the more strikes, the looser the processed structure. A laser beam overlap rate of ≤5% allows for better control of the final spacer region's morphology, forming a smoother, arched protrusion structure. In some embodiments, the overlap rate between any two laser beams can be 0% to 5%, for example, 0%, 0.5%, 0.8%, 1%, 1.2%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, or 5%.

[0094] In some specific embodiments of this application, each laser beam has the same power, and along the width direction of the interval, the number of laser strikes gradually decreases by 'a' times and then gradually increases by 'a' times, where 'a' can be 1 to 5, for example, 'a' can be 1, 2, 3, 4 or 5.

[0095] In some specific embodiments, the laser power remains constant, and the laser spot moves along the width of the interval (moving from left to right or from right to left). The first spot is hit n times, the second spot is hit n-1 times, and the overlap rate between the two laser spots is 0%. This continues until the spot in the middle of the interval is hit only once. The laser then continues to move to the right / left, and the number of times the spot is hit increases until it reaches the other side of the interval.

[0096] In some embodiments of this application, the energy of each laser beam applied to the spacer region is ≤50μJ, which is more conducive to controlling the looseness of the spacer region structure after laser treatment, resulting in a smoother arched protrusion structure after wet texturing.

[0097] In some specific embodiments, the laser power remains constant, the laser energy is 40 μJ, the laser spot moves along the width of the interval, the first spot is hit n times, the second spot is hit n-1 times, the overlap rate between the two laser spots is 0%, and so on until the spot in the middle of the interval is hit only once, and then it continues to move to the right / left, the number of times the spot is hit increases, until it reaches the other side of the interval.

[0098] S60: Perform wet texturing to remove the phosphorus silicate glass layer, n-type doped layer and part of the substrate on the spacer region, so that the substrate in the spacer region forms an arched protrusion structure.

[0099] Wet texturing is performed to remove the residual phosphosilicate glass layer, n-type doped layer, and part of the substrate (2 μm to 10 μm thick) and the n-type doped layer on the front side of the spacer region. An anisotropic pyramid structure is then formed in the spacer regions on both the front and back sides of the substrate. In some embodiments, the size of the pyramid structure can be 1.5 μm to 1.8 μm, and the height of the pyramid structure can be 0.6 μm to 1.2 μm.

[0100] In some embodiments of this application, when a second tunneling oxide layer is provided between the n-type doped layer and the substrate, the wet texturing step can remove the residual phosphosilicate glass layer, n-type doped layer, second tunneling oxide layer and part of the substrate (2μm to 10μm thickness), the n-type doped layer and the second tunneling oxide layer on the front side, and form a pyramid structure (anisotropic) in the spacer region on the front and back sides of the substrate.

[0101] In some embodiments of this application, the wet texturing process may involve pre-cleaning, followed by etching, and finally post-cleaning.

[0102] In some embodiments of this application, the cleaning solution used for pre-cleaning can be prepared at a volume ratio of alkali solution / hydrogen peroxide of 1:2 to 5, the pre-cleaning temperature can be 60°C to 70°C, and the pre-cleaning time can be 60s to 300s. The alkali in the alkali solution may include NaOH and / or KOH.

[0103] In some embodiments of this application, after pre-cleaning, an etching process is performed. The etching solution used in the etching process can be prepared according to an additive / alkali solution volume ratio of 1:2 to 4. The etching temperature can be 65°C to 85°C, and the etching time can be 100s to 500s. The alkali in the alkaline solution includes NaOH and / or KOH. In this application, the additive is a commercially available additive. The additive can complex with residual phosphorus oxides on the surface, slowing down the reaction rate. The more residual phosphorus oxides, the slower the reaction rate. By controlling the different PSG thicknesses in the laser-opened film area, the texturing speed at different positions in the interval area is controlled, ultimately forming an arched protrusion structure.

[0104] In some embodiments of this application, after the etching process, a post-cleaning is performed. The cleaning solution used for the post-cleaning can be prepared according to the volume ratio of alkaline solution / hydrogen peroxide of 1:2 to 5. The temperature of the post-cleaning can be 60°C to 70°C, and the time of the post-cleaning can be 60s to 300s. The alkali in the cleaning solution used for the post-cleaning can include NaOH and / or KOH.

[0105] In some embodiments of this application, after wet texturing to form an arched protrusion structure, the fabrication of the solar cell further includes the following steps: using an HF acid solution to remove the borosilicate glass layer in the first region and the phosphosilicate glass layer in the second region.

[0106] In some embodiments of this application, the fabrication of a solar cell further includes the following steps: forming a front passivation film and a back passivation film; forming a front antireflection film and a back antireflection film; printing and sintering the back electrode (first grid line and second grid line) to form an electrode system.

[0107] In some embodiments, the front passivation film and the back passivation film may each independently comprise an alumina passivation film. In some embodiments, the front antireflection film and the back antireflection film may each independently comprise a silicon nitride antireflection film.

[0108] In another aspect, this application proposes a photovoltaic module. In some embodiments of this application, the photovoltaic module may include the solar cell described above, or the photovoltaic module may include a solar cell prepared using the methods described above. Therefore, the photovoltaic module possesses all the features and advantages of the solar cell described above, which will not be repeated here. In general, the photovoltaic module has high light absorption capacity and high utilization rate of incident light.

[0109] In some embodiments of this application, a photovoltaic module may include multiple solar cells.

[0110] The present application will be described below through specific embodiments. Those skilled in the art will understand that the specific embodiments below are merely illustrative and do not limit the scope of the present application in any way. Furthermore, in the following embodiments, unless otherwise specified, the materials and equipment used are commercially available. If specific processing conditions and methods are not explicitly described in the later embodiments, conditions and methods known in the art can be used for processing.

[0111] Example 1

[0112] (1) Using an N-type single crystal silicon wafer as a substrate, the substrate is cleaned and polished to remove substrate slice damage and surface dirt to form a tower base.

[0113] The substrate includes a front side and a back side. The back side can be divided into a first region, a second region, and a spacer region. The first region is used to set a first functional structure with a p-type doped layer, the second region is used to set a second functional structure with an n-type doped layer, and the spacer region is used to separate the first functional structure and the second functional structure.

[0114] (2) The first tunneling oxide layer (silicon oxide) was grown on the surface of the substrate by LPCVD at a temperature of 600℃ for 10 min.

[0115] An intrinsic polycrystalline silicon layer was grown on the side of the first tunneling oxide layer away from the substrate using LPCVD at a growth temperature of 600℃ for 5 minutes.

[0116] (3) Boron diffusion was performed to dope the intrinsic polysilicon layer with boron to form a p-type doped layer (boron-doped polysilicon layer). The diffusion temperature was 850℃ and the diffusion time was 8 min. BSG was then formed by post-oxidation at 950℃ for 30 min.

[0117] (4) Laser grooving: A 532nm wavelength laser is used to create patterned grooves on the BSG on the back side. The laser-irradiated areas are the second region and the interval region.

[0118] (5) The front-side BSG is removed by a high-concentration HF acid solution of a chain machine. The concentration of the HF acid solution is 40%, the length of the acid tank is 4m, and the running speed is 2.5m / min.

[0119] (6) Wet etching to remove the borosilicate glass layer, p-type doped layer, first tunneling oxide layer and a small amount of substrate remaining in the back laser grooving area of ​​step (4), and the first tunneling oxide layer and a small amount of substrate on the front side, to form a tower base.

[0120] (7) A second tunneling oxide layer (silicon oxide) is grown on the back side using LPCVD at a temperature of 600°C for 10 minutes.

[0121] An intrinsic polycrystalline silicon layer was grown on the side of the second tunneling oxide layer away from the substrate using LPCVD at a growth temperature of 600℃ for 8 minutes.

[0122] (8) Phosphorus diffusion is performed to dope the intrinsic polycrystalline silicon layer with phosphorus to form an n-type doped layer (phosphorus-doped polycrystalline silicon layer). The diffusion temperature is 850℃ and the diffusion time is 25min. PSG is formed by post-oxidation at a temperature of 930℃ for 30min.

[0123] (9) Laser grooving: Laser grooving is performed on the first area and the interval area to remove PSG.

[0124] For the first region, a 532nm wavelength laser is used to irradiate the first region to remove the PSG in the region.

[0125] For the interval region, a 50μJ laser is used to process the region from left to right along the width of the interval region. The first laser spot is hit n times, the second laser spot is hit n-1 times, where n is between 3 and 8. The overlap rate between the two laser spots is 0%, and so on. The middle laser spot is hit only once. The process continues to move to the right, and the number of laser spot hits increases sequentially (the number of hits increases by 1 for each move to the right) until the other side of the interval region.

[0126] (10) The PSG on the front is removed by a high-concentration HF acid solution of a chain machine. The concentration of the HF acid solution is 20%, the length of the acid tank is 2m, and the running speed is 4.3m / min.

[0127] (11) Wet texturing: A cleaning solution is prepared at a volume ratio of alkali solution to hydrogen peroxide of 1:2 and used for pre-cleaning of the battery cells at a temperature of 65°C for 100 seconds. The alkali used is NaOH. An etching solution is prepared at a volume ratio of additive to alkali solution of 1:3 and used for etching at a temperature of 75°C for 200 seconds. The alkali used is NaOH. A cleaning solution is prepared at a volume ratio of alkali solution to hydrogen peroxide of 1:2 and used for post-cleaning of the battery cells at a temperature of 65°C for 100 seconds. The alkali used is NaOH.

[0128] The residual phosphorosilicate glass layer, n-type doped layer, second tunneling oxide layer, and a small amount of substrate, front-side n-type doped layer, and second tunneling oxide layer in the laser grooving area are removed by wet texturing, and a pyramid structure (anisotropic) is formed on the substrate.

[0129] (12) Use HF acid solution to remove the borosilicate glass layer in the first region and the phosphosilicate glass layer in the second region.

[0130] (13) Deposit aluminum oxide passivation films on the front and back sides.

[0131] (14) Deposit silicon nitride antireflective films on the front and back sides.

[0132] (15) Electrode printing and sintering are performed on the back side to form an electrode system and obtain a solar cell.

[0133] Example 2

[0134] Unlike Example 1, in step (9) of Example 2, the interval region is laser-grooved using a 40 μJ laser. The remaining steps and parameters are consistent with those of Example 1.

[0135] Example 3

[0136] Unlike Example 1, in step (9) of Example 3, when laser grooving is performed on the interval area, the number of hits of two adjacent laser spots differs by 3, while the middle spot is still hit only once. The remaining parameters and steps are consistent with those of Example 1.

[0137] Example 4

[0138] Unlike Example 1, in step (9) of Example 4, when laser grooving is performed on the interval area, the number of hits of two adjacent laser spots differs by 5, while the middle spot is still hit only once. The remaining parameters and steps are consistent with those of Example 1.

[0139] Example 5

[0140] Unlike Example 1, in step (9) of Example 5, when laser grooving is performed on the interval area, the middle laser spot is only fired once, and the overlap rate of two adjacent laser spots is 2%. The remaining parameters and steps are consistent with those of Example 1.

[0141] Example 6

[0142] Unlike Example 1, in step (9) of Example 6, when laser grooving is performed on the interval area, the middle laser spot is only fired once, and the overlap rate of two adjacent laser spots is 5%. The remaining parameters and steps are consistent with those of Example 1.

[0143] Example 7

[0144] Unlike Example 1, the laser grooving steps for the interval region are as follows: Along the width of the interval region, each laser spot strikes 10 times. The energy of the first spot is 50 μJ, the energy of the second spot is 45 μJ, and the overlap between the two laser spots is 0%. This continues, with the middle spot having the lowest energy. Moving to the right, the laser energy increases sequentially (by 5 μJ for each rightward movement) until the other side of the interval region is reached. The remaining parameters and steps are consistent with Example 1.

[0145] In each embodiment, by adjusting the parameters of laser grooving the spacer region in step (9), the looseness of the spacer region structure can be gradually reduced and then gradually increased along the width direction of the spacer region after laser grooving. During wet texturing, the looser the structure, the faster the etching solution reacts with it, ultimately forming an arched protrusion structure. The arched protrusion structure can significantly increase the area of ​​the textured surface on the back side, improve the light absorption capacity of the solar cell, and thus improve the cell efficiency.

[0146] In the description of this application, the terms "front", "back", etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are used only for the convenience of describing this application and do not require this application to be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this application.

[0147] In the description of this specification, the references to terms such as "one embodiment," "some embodiments," and "other embodiments" indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment is included in at least one embodiment of this application. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples. Moreover, those skilled in the art can combine and integrate the different embodiments or examples described in this specification, as well as the features of different embodiments or examples, without contradiction. Additionally, it should be noted that in this specification, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of indicated technical features.

[0148] Although embodiments of this application have been shown and described above, it is understood that the above embodiments are exemplary and should not be construed as limiting this application. Those skilled in the art can make changes, modifications, substitutions and variations to the above embodiments within the scope of this application.

Claims

1. A solar cell, wherein, The solar cell includes a substrate, which includes a front side and a back side disposed opposite to each other. The back side is divided into a first region, a second region, and a spacer region. A first functional structure is disposed on the first region, which includes a p-type doped layer. A second functional structure is disposed on the second region, which includes an n-type doped layer. The spacer region is used to separate the first functional structure and the second functional structure. Along the direction from the front to the back, the substrate of the spacer region has an arched protrusion structure.

2. The solar cell of claim 1, wherein, The height difference between the highest and lowest points of the arched protrusion structure is 1.5 μm to 7 μm.

3. The solar cell according to claim 1 or 2, wherein The height difference between the surface of the p-type doped layer away from the substrate and the highest point of the arched protrusion structure is ≥3μm.

4. The solar cell according to any one of claims 1 to 3, wherein The height difference between the surface of the n-type doped layer away from the substrate and the highest point of the arched protrusion structure is ≥1.5 μm.

5. A method of fabricating a solar cell, wherein, include: A substrate is provided, the substrate including a front side and a back side disposed opposite to each other, the back side being divided into a first region, a second region and a spacer region; A p-type doped layer and a borosilicate glass layer are formed on the back side; Remove the borosilicate glass layer and the p-type doped layer from the second region and the spacer region; An n-type doped layer and a phosphosilicate glass layer are formed on the back side; Laser processing is performed on the structures in the first region and the interval region, wherein the laser energy applied to the interval region along the width direction of the interval region first gradually decreases and then gradually increases; Wet texturing is performed to remove the phosphosilicate glass layer, the n-type doped layer, and part of the substrate on the spacer region, so that the substrate of the spacer region forms an arched protrusion structure.

6. The method of claim 5, wherein, Along the width of the interval, lasers are used to process different positions of the interval. Each laser beam strikes the same number of times, and the power of the laser gradually decreases and then gradually increases. The overlap rate between any two laser beams is ≤5%.

7. The method of claim 5, wherein, Along the width of the interval, a laser beam is used to laser process different positions of the interval. Each laser beam has the same power, and the number of laser strikes gradually decreases and then gradually increases. The overlap rate between the spots of any two laser beams is ≤5%.

8. The method of claim 7, wherein, Along the width of the interval, the number of laser strikes first gradually decreases by 'a' times and then gradually increases by 'a' times, where 'a' is 1 to 5.

9. The method according to any one of claims 5 to 8, wherein, At least one of the following conditions must be met: The energy of each laser beam applied to the interval region is ≤50 μJ; The etching solutions used in wet texturing include sodium hydroxide and / or potassium hydroxide; The arched protrusion structure has multiple pyramid structures, the size of which is 1.5μm to 1.8μm and the height of which is 0.6μm to 1.2μm.

10. A photovoltaic module, wherein, The solar cell includes any one of claims 1 to 4, or a solar cell prepared using any one of claims 5 to 9.