Organometallic compound and organic electroluminescent device comprising same
By introducing specific substituents into organometallic compounds and optimizing their electron cloud density and conjugation degree, the problems of high voltage and short lifetime in organic light-emitting devices have been solved, realizing high-efficiency and long-life organic electroluminescent devices.
Patent Information
- Application Number
- PCT/CN2025/119638
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-12
- Filing Date
- 2025-09-08
- Publication Date
- 2026-11-19
AI Technical Summary
Existing organic light-emitting devices suffer from high voltage and short lifespan. Developing high-efficiency, long-lifespan, and low-voltage organic materials is an urgent technical problem to be solved.
An organometallic compound is used as a light-emitting layer material for organic electroluminescent devices by introducing specific substituents, such as methyl, ethyl, phenyl, and fluorine groups, into its structure to optimize its conjugation degree and electron cloud density.
It significantly improves the stability and lifetime of organic electroluminescent devices, reduces the driving voltage, and increases the maximum external quantum efficiency.
Smart Images

Figure CN2025119638_19112026_PF_FP_ABST
Abstract
Description
An organometallic compound and an organic electroluminescent device comprising the same. Technical Field
[0001] This invention belongs to the field of organic optoelectronic materials, specifically relating to an organometallic compound and an organic electroluminescent device containing the same. Background Technology
[0002] Organic light emission typically refers to the phenomenon of converting electrical energy into light energy using organic materials. Organic light-emitting devices (OLEDs) utilizing organic light emission exhibit characteristics such as wide viewing angle, excellent contrast ratio, fast response time, and superior brightness, driving voltage, and response speed.
[0003] Organic light-emitting devices (OLEDs) typically have a structure comprising an anode, a cathode, and an organic material layer between the anode and cathode. The organic material layer often has a multilayer structure comprising different materials to improve the efficiency and stability of the OLED. For example, the organic material layer can be formed from a hole injection layer, a hole transport layer, a light-emitting layer, an electron transport layer, and an electron injection layer. In the structure of an OLED, if a voltage is applied between the two electrodes, holes are injected into the organic material layer from the anode, and electrons are injected into the organic material layer from the cathode. When the injected holes and electrons meet, excitons are formed, and light is emitted when the excitons return to their ground state.
[0004] The light-emitting layer significantly affects the efficiency and performance of organic light-emitting devices (OLEDs), making the development of novel light-emitting materials that meet practical requirements crucial. However, due to the complex, time-consuming, and short-lifespan synthesis process of phosphorus-based materials, developing a high-performance organic material that enables OLEDs to achieve high efficiency, long lifespan, and low voltage is a pressing technical problem that needs to be solved by researchers in this field. Summary of the Invention
[0005] To address the shortcomings of existing technologies, this invention discloses an organometallic compound and an organic electroluminescent device comprising the same.
[0006] To achieve the above objectives, the following technical solution is adopted:
[0007] The first objective of this invention is to provide an organometallic compound having the structure shown in general formula I:
[0008] Among them, at least one of R1, R2, R3 and R4 is not hydrogen, and each is independently selected from hydrogen, deuterium, fluorine, cyano, isocyano, methyl, ethyl, n-propyl, isopropyl, isobutyl, n-butyl, tert-butyl, sec-butyl, isopentyl, neopentyl, phenyl;
[0009] The following groups are replaced by deuterium or fluorine: methyl, ethyl, n-propyl, isopropyl, isobutyl, n-butyl, tert-butyl, sec-butyl, isopentyl, neopentyl;
[0010] The following groups, substituted or unsubstituted by deuterium, fluorine, -CD3, methyl, ethyl, isopropyl, n-propyl, n-butyl, sec-butyl, isobutyl, tert-butyl, isopentyl, octylpentyl, or phenyl, biphenyl, and combinations thereof;
[0011] R5, R6, R7 and R8 include at least two that are not hydrogen, and each is independently selected from hydrogen, deuterium, fluorine, cyano, isocyano, methyl, ethyl, n-propyl, isopropyl, isobutyl, n-butyl, tert-butyl, sec-butyl, isopentyl, neopentyl, phenyl;
[0012] The following groups, substituted with deuterium or fluorine, include: methyl, ethyl, n-propyl, isopropyl, isobutyl, n-butyl, tert-butyl, sec-butyl, isopentyl, neopentyl, and...
[0013] n is an integer selected from 0 to 5 (e.g., 0, 1, 2, 3, 4, 5), and R' is selected from the following groups: deuterium, fluorine, -CD3, methyl, ethyl, isopropyl, n-propyl, n-butyl, sec-butyl, isobutyl, tert-butyl, isopentyl, octylpentyl.
[0014] R9, R 10 R 11 R 12 R 13 R 14 R 15 and R 16 Each is independently selected from hydrogen, deuterium, fluorine, cyano, substituted or unsubstituted C1-C15 alkyl, substituted or unsubstituted C3-C18 cycloalkyl, substituted or unsubstituted C6-C18 aryl and combinations thereof;
[0015] R 17 and R 18 Each is independently selected from hydrogen, deuterium, fluorine, methyl, and -CD3;
[0016] R 19 and R 20 Each is independently selected from fluorine, methyl or deuterated methyl, ethyl or deuterated ethyl.
[0017] It should be noted that R9-R 16In the definition of "substituted or unsubstituted", substitution refers to substitution by one or at least two substituents selected from the following, or at least two connected substituents: hydrogen, deuterium, fluorine, cyano, trifluoromethyl, methyl, ethyl, -CD3, -CF3, -CH2F, -CHF2, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, sec-butyl, 1-methylbutyl, 1-ethylbutyl, n-pentyl, isopentyl, neopentyl, tert-pentyl, n-hexyl, 1-methylpentyl, 2-methylpentyl, 4-methyl-2-pentyl, 3,3-dimethylbutyl, 2-ethylbutyl, 1-methylhexyl, phenyl, biphenyl, naphthyl, anthracene, phenanthrene, thiophene, furanyl, pyrrole, benzothiophene, benzofuranyl, pyridyl, indolyl, cyclopentyl, cyclohexyl, or adamantyl. The phrase "at least two connected substituents" refers to groups obtained by further substituting and connecting at least two of the aforementioned substituents. For example, for methyl and phenyl, the connected substituents can be methylphenyl or benzyl.
[0018] Furthermore, Equation I is selected from Equations II-VII:
[0019] Furthermore, at least one of R1-R4 is not hydrogen, and each is independently selected from hydrogen, deuterium, fluorine, cyano, methyl, ethyl, isopropyl, isobutyl, tert-butyl, isopentyl, neopentyl, phenyl, methylphenyl, -CD3, and the following groups;
[0020] R9, R 10 R 11 R 12 R 13 R 14 R 15 and R 16 Each group is independently selected from hydrogen, methyl, ethyl, fluoro, cyano, -CD3, tert-butyl, isopropyl, n-propyl, and the following groups:
[0021] It should be noted that the compounds represented by Formula I can be used as materials in the organic material layer of organic electroluminescent devices, and can improve efficiency, achieve low driving voltage, and improve lifetime characteristics in organic electroluminescent devices. In particular, the compounds represented by Formula I can be used as materials in the light-emitting layer.
[0022] Preferably, ligand Preferred selections are from the following structures LA-1 to LA-95:
[0023] In the above technical solution, the organometallic compound is preferably selected from any one of the following structures:
[0024] The above are just some specific structural forms, but this series of organometallic compounds is not limited to the above molecular structures. Other specific molecular structures can be obtained by simply changing some simple groups and their substituted groups and substitution positions, which will not be elaborated here.
[0025] The organometallic compounds represented by Formula I have a maximum emission wavelength of 500 nm to 560 nm, which enables the prepared organometallic compounds to significantly improve stability, increase lifespan and reduce driving voltage when used in organic electroluminescent devices.
[0026] Furthermore, this invention also claims protection for a method for preparing the above-mentioned organometallic compound, as follows:
[0027] Synthesis of intermediate TM4:
[0028] Step 1: Add raw material A (1 eq), raw material B (1.02-1.05 eq), anhydrous potassium carbonate (1.5-2 eq), and N,N-dimethylformamide (15 eq) to the reactor, replace with nitrogen, heat to 140℃-150℃, stir and react for 4-6 hours, then cool to room temperature, add water to the reaction system, filter, and purify the filter cake with ethanol and petroleum ether to obtain intermediate TM1;
[0029] Step 2: Add intermediate TM1 (1 eq) and N,N-dimethylformamide (10 eq) to the reactor, replace with nitrogen, and under nitrogen protection, add palladium acetate (0.02-0.1 eq) and tricyclohexylphosphine (0.02-0.1 eq) to the system, replace with nitrogen, heat to 150-160℃, react for 4-6 hours, and when the liquid phase monitoring shows that there is basically no raw material remaining, stop heating, cool to room temperature, add water to the reaction system, filter, and purify the filter cake with ethanol or ethyl acetate to obtain intermediate TM2;
[0030] Step 3: Add intermediate TM2 (1 eq), pinacol diborate (2 eq), potassium acetate (2.5 eq), and 1,4-dioxane (40 eq) to the reactor, replace with nitrogen, and under nitrogen protection, add bis(dibenzylacetone)palladium (0.02 eq) and 2-dicyclohexylphosphine-2',4',6'-triisopropylbiphenyl (X-Phos) (0.08 eq) to the system. React at 80-90℃ for 10-12 hours. After the reaction is complete, evaporate the reaction solution to dryness, pass it through a silica gel funnel, and perform column chromatography. Use petroleum ether and dichloromethane as eluents, concentrate, and obtain intermediate TM3.
[0031] Step 4: Weigh intermediate TM3 (1 eq), raw material C (1.2 eq), anhydrous potassium carbonate (3 eq), toluene (10 eq), ethanol (5 eq), and water (10 eq) and add them to the reactor. Replace the nitrogen gas. Under nitrogen protection, add tetra(triphenylphosphine)palladium (0.03 eq) to the system and react at 80-90℃ for 10-12 hours. After the reaction is complete, allow the mixture to stand and separate the liquids. Combine the organic phases, pass them through a silica gel funnel, and perform column chromatography. Use petroleum ether and ethyl acetate as eluents. Concentrate the mixture to obtain intermediate TM4.
[0032] Synthesis of Formula I:
[0033] Step 5: Weigh raw material D (2.2 eq), IrC13·3H2O (1 eq), ethylene glycol ethyl ether (20 eq), and water (6.5 eq) and add them to the reactor. Replace the nitrogen gas and reflux the reaction at 110℃~120℃ for 40-48 hours. After the reaction is completed, cool to room temperature. A precipitate will form. Filter the precipitate and wash it with anhydrous ethanol and petroleum ether in sequence and dry it to obtain the bridged ligand D-1.
[0034] Step 6: Weigh the bridging ligand D-1 (1 eq), silver trifluoromethanesulfonate (2.2 eq), dichloromethane (20 eq), and methanol (4 eq) and add them to the reactor. Under nitrogen protection, react at room temperature for 40-48 hours. After the reaction is complete, pass the mixture through a silica gel funnel and evaporate to dryness to obtain intermediate D-2.
[0035] Step 7: Weigh intermediate D-2 (1 eq), intermediate TM4 (2.5 eq), and anhydrous ethanol (15 eq) and add them to the reactor. Replace the nitrogen gas and react at 80-90℃ for 40-48 hours. After the reaction is complete, cool to room temperature. A precipitate will form. Filter the precipitate, wash the filter cake with ethanol and petroleum ether, dry it, and perform column chromatography. Use petroleum ether and dichloromethane as eluents. Concentrate the filtrate to obtain organometallic compound I.
[0036] The second technical objective of this invention is to provide an organic electroluminescent device, the organic electroluminescent device comprising an organic layer; the organic layer comprising an organometallic compound as described above.
[0037] Specifically, the organometallic compound can be in a single form or it can exist mixed with other substances in the organic layer.
[0038] Furthermore, the organic electroluminescent device further includes a first electrode and a second electrode; the organic layer is located between the first electrode and the second electrode; wherein the organic layer includes a light-emitting layer, and the light-emitting layer contains an organometallic compound as described above.
[0039] Furthermore, the light-emitting layer comprises a host material and a dopant material; the dopant material comprises the organometallic compound as described above; and the mass ratio of the host material to the dopant material is (10-99.5):0.5 (e.g., 10:0.5, 20:0.5, 30:0.5, 40:0.5, 50:0.5, 60:0.5, 70:0.5, 80:0.5, 90:0.5, 95:0.5, 99:0.5, 99.5:0.5).
[0040] Generally, the organic layer also includes one or more of the following: a hole injection layer, a hole transport layer, a layer that has both hole injection and hole transport functions, an electron blocking layer, a hole blocking layer, an electron transport layer, an electron injection layer, and a layer that has both electron transport and electron injection functions; wherein at least one functional layer contains the organometallic compound described in this invention.
[0041] Furthermore, this invention also provides the application of an organic electroluminescent device in the fabrication of organic light-emitting devices, organic solar cells, electronic paper, organic photoreceptors, or organic thin-film transistors. By introducing organometallic compounds into the light-emitting layer, the device is endowed with superior performance.
[0042] As can be seen from the above technical solution, compared with the prior art, the present invention has the following beneficial effects:
[0043] 1) Introduce at least two substituents onto the monoligand pyridine ring to change the activity of the substituents, thereby making the resulting organometallic compound more stable; 2) Introduce at least one functional group onto the monoligand benzene ring (R1, R2, R3, R4) to change the degree of conjugation of the system, thereby delaying the lifetime, reducing the driving voltage, and improving the maximum external quantum efficiency of the resulting organometallic compound when used in organic electroluminescent devices. Attached Figure Description
[0044] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on the provided drawings without creative effort.
[0045] Figure 1 shows the 1H NMR spectrum of compound G-100 prepared in Example 1. Detailed Implementation
[0046] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments and related drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0047] This invention specifically discloses an organometallic compound, its preparation method, and an organic electroluminescent device.
[0048] The features and performance of the present invention will be further described in detail below with reference to specific embodiments.
[0049] Example 1: Preparation of G-100
[0050] raw material The synthesis method of (CAS:2718130-10-8) is cited in patent literature: CN113121584A, SCI literature DOI: 10.1002 / anie.201504066.
[0051] Step 1: Weigh 1-hydroxy-5,5-dimethylsilylfluorene (1 eq), 1-bromo-3-chloro-2-fluorobenzene (CAS: 144584-65-6, 1.02 eq), anhydrous potassium carbonate (1.5 eq), and N,N-dimethylformamide (15 eq) sequentially into a reactor, purge with nitrogen, heat to 145°C, stir for 4 hours, then cool to room temperature, add water to the reaction system, filter, and purify the filter cake with ethanol and petroleum ether to obtain intermediate S1, with a yield of 66.92%.
[0052] HPLC: ≥99.2%.
[0053] Mass spectrometry: Test value 414.12.
[0054] Step 2: Weigh S1 (1 eq) and N,N-dimethylformamide (10 eq) and add them to the reactor. Replace the nitrogen gas. Under nitrogen protection, add palladium acetate (0.02 eq) and tricyclohexylphosphine (0.02 eq) to the system, replace the nitrogen gas, heat to 160°C, and react for 4 hours. When the liquid phase monitoring shows that there is basically no raw material remaining, stop heating, cool to room temperature, add water to the reaction system, filter, and purify the filter cake with ethanol or ethyl acetate to obtain intermediate S2 with a yield of 56.7%.
[0055] HPLC: ≥99.2%.
[0056] Mass spectrometry: Test value 334.26.
[0057] Step 3: Weigh S2 (1 eq), pinacol diborate (2 eq), potassium acetate (2.5 eq), and 1,4-dioxane (40 eq) and add them to the reactor. Replace the nitrogen gas. Under nitrogen protection, add bis(dibenzylacetone)palladium (0.02 eq) and 2-dicyclohexylphosphine-2',4',6'-triisopropylbiphenyl (X-Phos) (0.08 eq) to the system. React at 80°C for 12 hours. After the reaction is complete, evaporate the reaction solution to dryness, pass it through a silica gel funnel, and perform column chromatography. Use petroleum ether and dichloromethane as eluents. Concentrate to obtain intermediate S3 with a yield of 75.25%.
[0058] HPLC: ≥99%.
[0059] Mass spectrometry: Test value 426.35.
[0060] Step 4: Weigh 2-bromo-4-chloro-5-methylpyridine (1 eq), intermediate S3 (1.1 eq), anhydrous potassium carbonate (3 eq), toluene (10 eq), ethanol (5 eq), and water (10 eq) and add them to the reactor. Replace the nitrogen atmosphere. Under nitrogen protection, add tetra(triphenylphosphine)palladium (0.03 eq) to the system. React at 85°C for 12 hours. After the reaction is complete, allow to stand and separate the liquids. Combine the organic phases, pass through a silica gel funnel, and perform column chromatography. Elute with petroleum ether and ethyl acetate. Concentrate to obtain intermediate S4, with a yield of 73.12%.
[0061] HPLC: ≥99.5%.
[0062] Mass spectrometry: Test value 425.28.
[0063] Step 5: Weigh 1-bromo-4-isobutylbenzene (1 eq), pinacol diborate (2 eq), potassium acetate (2.5 eq), and 1,4-dioxane (40 eq) and add them to the reactor. Replace the nitrogen gas. Under nitrogen protection, add bis(dibenzylacetone)palladium (0.02 eq) and X-Phos (0.08 eq) to the system. React at 80°C for 12 hours. After the reaction is complete, evaporate the reaction solution to dryness, pass it through a silica gel funnel, and perform column chromatography. Use petroleum ether and dichloromethane as eluents. Concentrate to obtain intermediate S5 with a yield of 69%.
[0064] HPLC: ≥99%.
[0065] Mass spectrometry: Test value 260.31.
[0066] Step 6: Weigh intermediate S4 (1 eq), intermediate S5 (1.2 eq), anhydrous potassium carbonate (3 eq), toluene (10 eq), ethanol (5 eq), and water (10 eq) and add them to the reactor. Replace the nitrogen atmosphere. Under nitrogen protection, add tetrakis(triphenylphosphine)palladium (0.03 eq) to the system. React at 80°C for 10 hours until the reaction is complete. Allow the mixture to stand, separate the liquids, combine the organic phases, pass them through a silica gel funnel, and perform column chromatography. Elute with petroleum ether and ethyl acetate, concentrate, and obtain intermediate S6 in 70.52% yield.
[0067] HPLC: ≥99.5%.
[0068] Mass spectrometry: Test value 523.45.
[0069] Step 7: Weigh intermediate S6 (1 eq) and tetrahydrofuran (THF, 40 eq). When the internal temperature of the system is lowered to -78℃, slowly add diisopropylaminolithium (2.5 eq, 2 mol / L) dropwise to the system. During the dropwise addition, control the internal temperature between -76℃ and -80℃. After the dropwise addition is complete, keep the system at -78℃ for 3 hours. Then slowly add heavy water (50 eq) dropwise to the system. After the dropwise addition is complete, allow the system to rise naturally to room temperature and react for 8 hours. Add 5 L of saturated sodium chloride solution and 7 L of ethyl acetate to the system. Separate the solution, concentrate, and perform column chromatography. Use dichloromethane and ethyl acetate as eluents. Concentrate to obtain intermediate S6-2 with a yield of 38.73%.
[0070] HPLC: ≥99.5%.
[0071] Mass spectrometry: Test value 524.31.
[0072] Step 8: Weigh 2-phenylpyridine (2.2 eq), IrC13·3H2O (1 eq), ethylene glycol ethyl ether (20 eq), and water (6.5 eq) and add them to the reactor. Replace the nitrogen gas and reflux at 120°C for 48 hours. After the reaction is complete, cool to room temperature. A precipitate will form. Filter the precipitate and wash it with anhydrous ethanol and petroleum ether in sequence. Dry the precipitate to obtain the bridged ligand S7 with a yield of 89.65%.
[0073] Step 9: Weigh the bridging ligand S7 (1 eq), silver trifluoromethanesulfonate (2.2 eq), dichloromethane (20 eq), and methanol (4 eq) and add them to the reactor. Under nitrogen protection, react at room temperature for 48 hours. After the reaction is complete, pass the mixture through a silica gel funnel and evaporate to dryness to obtain intermediate S8, with a yield of 92.14%.
[0074] Step 10: Weigh intermediate S8 (1 eq), intermediate S6-2 (2.5 eq), and anhydrous ethanol (15 eq) and add them to the reactor. Replace with nitrogen and react at 80°C for 48 hours. After the reaction is complete, cool to room temperature. A precipitate will form. Filter the precipitate and wash the filter cake with ethanol and petroleum ether. Dry the cake and perform column chromatography using petroleum ether and dichloromethane as eluents. Concentrate the filtrate to obtain organometallic compound G-100 with a yield of 24.75%.
[0075] HPLC: ≥99.2%.
[0076] Mass spectrometry: Test value 1024.43.
[0077] See attached figure 1 for the NMR results.
[0078] Example 2 Preparation of G-102
[0079] Step 1: Weigh 2-bromo-4-chloro-5-methylpyridine (1 eq), sodium hydroxide (27 eq), and deuterated dimethyl sulfoxide (40 eq) and add them to the reactor. Replace with nitrogen gas and react at 85°C for 36 hours. After the reaction is complete, separate the solutions, perform column chromatography, eluent with dichloromethane, and concentrate to obtain intermediate S9 in 68.75% yield.
[0080] HPLC: ≥99.8%.
[0081] Mass spectrometry: Test value 208.05.
[0082] Step 2: Weigh intermediate S3 (1.0 eq), intermediate S9 (1.2 eq), anhydrous potassium carbonate (3 eq), toluene (10 eq), ethanol (5 eq), and water (10 eq) and add them to the reactor. Replace the nitrogen gas. Under nitrogen protection, add tetra(triphenylphosphine)palladium (0.03 eq) and react at 85°C for 12 hours. After the reaction is complete, allow the mixture to stand and separate the liquids. Combine the organic phases and pass them through a silica gel funnel for column chromatography. Use petroleum ether and ethyl acetate as eluents. Concentrate to obtain intermediate S10 with a yield of 68.45%.
[0083] HPLC: ≥99.2%.
[0084] Mass spectrometry: Test value 428.33.
[0085] Step 3: Weigh 1-chloro-2-methyl-4-neopentylbenzene (1 eq), potassium hydroxide (2.5 eq), and deuterated dimethyl sulfoxide (40 eq) and add them to the reactor. Replace with nitrogen gas and reflux at 90°C for 48 hours. After the reaction is complete, separate the liquid and perform column chromatography with dichloromethane and ethyl acetate as eluents. Concentrate to obtain intermediate S11 with a yield of 59.65%.
[0086] HPLC: ≥99.8%.
[0087] Mass spectrometry: Test value 201.25.
[0088] Step 4: Weigh intermediate S11 (1 eq), pinacol diborate (2 eq), potassium acetate (2.5 eq), and 1,4-dioxane (40 eq) and add them to the reactor. Replace the nitrogen gas. Under nitrogen protection, add bis(dibenzylacetone)palladium (0.02 eq) and X-Phos (0.08 eq) to the system. React at 80°C for 12 hours. After the reaction is complete, evaporate the reaction solution to dryness, pass it through a silica gel funnel, and perform column chromatography. Use petroleum ether and dichloromethane as eluents. Concentrate to obtain intermediate S12 with a yield of 73.25%.
[0089] HPLC: ≥99%.
[0090] Mass spectrometry: Test value 293.44.
[0091] Step 5: Weigh intermediate S10 (1 eq), intermediate S12 (1.2 eq), anhydrous potassium carbonate (3 eq), toluene (10 eq), ethanol (5 eq), and water (10 eq) and add them to the reactor. Replace the nitrogen gas. Under nitrogen protection, add tetra(triphenylphosphine)palladium (0.03 eq) to the system and react at 80°C for 10 hours. After the reaction is complete, allow the mixture to stand and separate the liquids. Combine the organic phases, pass them through a silica gel funnel, and perform column chromatography. Use petroleum ether and ethyl acetate as eluents. Concentrate to obtain intermediate S13 with a yield of 73.11%.
[0092] HPLC: ≥99.7%.
[0093] Mass spectrometry: Test value 559.44.
[0094] Step 6: Weigh intermediate S13 (1 eq) and tetrahydrofuran (THF, 40 eq). When the internal temperature of the system is lowered to -78℃, slowly add diisopropylaminolithium (2.5 eq, 2 mol / L) dropwise to the system. During the dropwise addition, control the internal temperature between -76℃ and -80℃. After the dropwise addition is complete, keep the system at -78℃ for 3 hours. Then slowly add heavy water (50 eq) dropwise to the system. After the dropwise addition is complete, allow the system to rise naturally to room temperature and react for 8 hours. Add 5 L of saturated sodium chloride solution and 7 L of ethyl acetate to the system. Separate the solution, concentrate, and perform column chromatography. Use dichloromethane and ethyl acetate as eluents. Concentrate to obtain intermediate S13-2 with a yield of 38.56%.
[0095] HPLC: ≥99.6%.
[0096] Mass spectrometry: Test value 560.12.
[0097] Step 7: Weigh 2-phenyl-5-methylpyridine (2.2 eq), IrC13·3H2O (1 eq), ethylene glycol ethyl ether (20 eq), and water (6.5 eq) and add them to the reactor. Replace the nitrogen gas and reflux at 120°C for 48 hours. After the reaction is complete, cool to room temperature. A precipitate will form. Filter the precipitate and wash it with anhydrous ethanol and petroleum ether in sequence. Dry the precipitate to obtain the bridged ligand S14 with a yield of 88.96%.
[0098] Step 8: Weigh the bridging ligand S14 (1 eq), silver trifluoromethanesulfonate (2.2 eq), dichloromethane (20 eq), and methanol (4 eq) and add them to the reactor. Under nitrogen protection, react at room temperature for 48 hours. After the reaction is complete, pass the mixture through a silica gel funnel and evaporate to dryness to obtain intermediate S15, with a yield of 94.15%.
[0099] Step 9: Weigh intermediate S15 (1 eq), intermediate S13-2 (2.5 eq), and anhydrous ethanol (15 eq) and add them to the reactor. Replace with nitrogen and react at 80°C for 48 hours. After the reaction is complete, cool to room temperature. A precipitate will form. Filter the precipitate and wash the filter cake with ethanol and petroleum ether. Dry the cake and perform column chromatography using petroleum ether and dichloromethane as eluents. Concentrate the filtrate to obtain organometallic compound G-102 with a yield of 33.25%.
[0100] HPLC: ≥99.3%.
[0101] Mass spectrometry: 1094.56.
[0102] 1 ¹H NMR (500 MHz, deuterated chloroform) δ 8.45 (s, 1H), 8.38 (d, 2H), 8.14–8.08 (m, 3H), 7.98–7.92 (m, 2H), 7.84 (d, 2H), 7.75 (dd, 1H), 7.69 (dd, 2H), 7.68–7.60 (m, 2H), 7.56–7.50 (m, 1H), 7.48 (d, 1H), 7.40 (s, 1H), 7.38–7.32 (m, 3H), 7.25–7.21 (m, 1H), 7.21–7.16 (m, 3H), 7.16–7.10 (m, 1H), 1.15 (s, 9H), 0.52 (s, 6H).
[0103] The preparation methods for other organometallic compounds are basically the same as those in the above examples, and will not be described in detail here.
[0104] To further describe the present invention, more specific embodiments are listed below:
[0105] Device Example 1: Fabrication of an organic electroluminescent device containing compound G-100
[0106] The ITO glass substrate with a coating thickness of 150nm was washed three times with distilled water, ultrasonically cleaned for 20 minutes, repeatedly washed three times with distilled water, ultrasonically cleaned for 15 minutes, and after the distilled water cleaning was completed, it was ultrasonically cleaned in sequence with solvents such as isopropanol, acetone, and methanol, and then dried. It was then transferred to a plasma cleaning machine, cleaned for 10 minutes, and sent to a vapor deposition machine.
[0107] 1) Vacuum evaporation of 70nm HI on ITO (anode) as a hole injection layer;
[0108] 2) A 70 nm N,N'-diphenyl-N,N'-(1-naphthyl)-1,1'-biphenyl-4,4'-diamine (i.e., NPB) was vacuum-deposited on the hole injection layer as a hole transport layer;
[0109] 3) A light-emitting layer is vacuum-deposited on the hole transport layer. The main material of the light-emitting layer, 4,4'-N,N'-dicarbazole biphenyl (CBP), and the dopant compound G-100 are mixed in a weight ratio of 90:10 and deposited at a depth of 40 nm to form the light-emitting layer.
[0110] 4) Vacuum evaporation of 20nm BAlq on the light-emitting layer to form a hole blocking layer;
[0111] 5) A 50 nm thick Alq3 layer was vacuum-deposited on the hole blocking layer as an electron transport layer;
[0112] 6) A 0.2 nm thick LiF layer was vacuum-deposited on the electron transport layer as an electron injection layer;
[0113] 7) An electroluminescent device was prepared by vacuum evaporating 150 nm of Al onto the electron injection layer as a cathode. Under constant brightness conditions, the performance and luminescence characteristics of the obtained electroluminescent device were tested to evaluate the driving voltage, maximum external quantum efficiency, and phosphorescence lifetime.
[0114] The material structure used in the device of this invention is shown below:
[0115] Device Examples 2-43
[0116] Organic electroluminescent devices of Device Examples 2-43 were prepared according to the preparation method of the organic electroluminescent device in Device Example 1, with the difference being that compound G-100 in Device Example 1 was replaced with G-1; G-3; G-8; G-19; G-21; G-24; G-56; G-66; G-82; G-101; G-102; G-106; G-126; G-145; G-159; G-185; G-205, respectively. G-222; G-237; G-238; G-255; G-269; G-290; G-297; G-308; G-350; G-369; G-406; G-428; G-430; G-435; G-451; G-455; G-476; G-477; G-489; G-497; G-502; G-519; G-550; G-552; G-565 form doped material compounds.
[0117] Comparative Examples 1-12
[0118] Organic electroluminescent devices of Comparative Examples 1-12 were prepared according to the preparation method of organic electroluminescent device in Device Example 1, except that: compound G-100 in Device Example 1 was replaced with Comparative Examples 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, and 12, respectively, to form doped material compounds.
[0119] The prepared organic electroluminescent device was subjected to the same testing as in Device Example 1, and the results are shown in Table 1.
[0120] Table 1
[0121] As can be seen from Table 1, the organometallic compounds provided by this invention, as the light-emitting layer materials for organic electroluminescent devices, can significantly reduce the driving voltage of organic electroluminescent devices, improve the lifetime of organic electroluminescent devices, and significantly enhance the external quantum efficiency compared to existing light-emitting layer materials (such as Comparative Examples 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, and 12).
[0122] 1) By introducing electron-donating groups (such as methyl, ethyl, isopropyl, tert-butyl, etc.) at different positions of the single ligand, the electron cloud density is increased, which raises the HOMO (highest occupied molecular orbital) energy level and the LUMO (lowest unoccupied molecular orbital) energy level. However, the HOMO energy level increases more significantly, resulting in a smaller band gap and a possible red shift in the emission spectrum. This leads to a better driving voltage for the organic electroluminescent device prepared using the compound of this invention compared to the driving voltage of the organic electroluminescent device prepared in the comparative example, resulting in improved luminous efficiency and significantly extended lifetime.
[0123] 2) By introducing electron-withdrawing groups (such as phenyl, substituted phenyl, etc.) at different positions of the single ligand, the phenyl group has a large conjugated system, and its introduction can significantly expand the degree of conjugation of the molecule, thus making the obtained compound more stable, resulting in a decrease in its electron cloud density, a decrease in the LUMO (lowest unoccupied molecular orbital) energy level, a larger band gap, and a possible red shift or blue shift in the emission spectrum. This leads to a significant reduction in the driving voltage and a significant improvement in the luminous efficiency of the organic electroluminescent device prepared using the compound of this invention.
[0124] 3) By introducing electron-withdrawing groups (such as fluorine or cyano groups) at different positions of the single ligand, the intermolecular forces are enhanced, the molecular arrangement becomes more ordered, and the stability of the compound is improved. The strong electron-withdrawing effect of fluorine lowers the LUMO energy level, increases the band gap, causes a blue shift in the emission spectrum, and improves the luminescence efficiency. It also leads to a significant reduction in the driving voltage and a delay in the lifetime of organic electroluminescent devices prepared using the compounds of this invention.
[0125] 4) By introducing deuterium atoms and deuterated groups (such as -D, -CD3, -CD2CD3, -CD2CH3, etc.) at different positions of the single ligand, the large mass of deuterium will reduce the vibrational frequency of the molecule, enhance the rigidity of the molecular structure, reduce non-radiative transition orbitals, and improve luminescence efficiency, resulting in a reduction in the driving voltage of organic electroluminescent devices prepared using the compounds of this invention.
[0126] The above description of the disclosed embodiments enables those skilled in the art to make or use the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. An organometallic compound characterized in that, The structure of the organometallic compound is shown in Formula I: Among them, at least one of R1, R2, R3 and R4 is not hydrogen, and each is independently selected from hydrogen, deuterium, fluorine, cyano, isocyano, methyl, ethyl, n-propyl, isopropyl, isobutyl, n-butyl, tert-butyl, sec-butyl, isopentyl, neopentyl, phenyl; The following groups are replaced by deuterium or fluorine: methyl, ethyl, n-propyl, isopropyl, isobutyl, n-butyl, tert-butyl, sec-butyl, isopentyl, neopentyl; The following groups, substituted or unsubstituted by one or more of deuterium, fluorine, -CD3, methyl, ethyl, isopropyl, n-propyl, n-butyl, sec-butyl, isobutyl, tert-butyl, isopentyl or octylpentyl: phenyl, biphenyl, and combinations thereof; R5, R6, R7 and R8 include at least two that are not hydrogen, and each is independently selected from hydrogen, deuterium, fluorine, cyano, isocyano, methyl, ethyl, n-propyl, isopropyl, isobutyl, n-butyl, tert-butyl, sec-butyl, isopentyl, neopentyl, phenyl; methyl, ethyl, n-propyl, isopropyl, isobutyl, n-butyl, tert-butyl, sec-butyl, isoamyl, neopentyl, and n is selected from an integer from 0 to 5, R' is selected from the group consisting of: deuterium, fluorine, -CD3, methyl, ethyl, isopropyl, n-propyl, n-butyl, sec-butyl, isobutyl, t-butyl, isoamyl, 2-pentyl, R9, R 10 , R 11 , R 12 , R 13 , R 14 , R 15 , and R 16 are each independently selected from the group consisting of hydrogen, deuterium, fluorine, cyano, substituted or unsubstituted C1-C15alkyl, substituted or unsubstituted C3-C18cycloalkyl, substituted or unsubstituted C6-C18aryl, and combinations thereof; R 17 and R 18 each independently is selected from hydrogen, deuterium, fluorine, methyl, -CD3; R 19 and R 20 each independently is selected from fluorine, methyl or deuterated methyl, ethyl or deuterated ethyl.
2. The organometallic compound according to claim 1, characterized in that, R9-R 16 In the definition of "substituted or unsubstituted", substitution refers to substitution by one or at least two substituents selected from the following, or at least two connected substituents: hydrogen, deuterium, fluorine, cyano, trifluoromethyl, methyl, ethyl, -CD3, -CF3, -CH2F, -CHF2, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, sec-butyl, 1-methylbutyl, 1-ethylbutyl, n-pentyl, isopentyl, neopentyl, tert-pentyl, n-hexyl, 1-methylpentyl, 2-methylpentyl, 4-methyl-2-pentyl, 3,3-dimethylbutyl, 2-ethylbutyl, 1-methylhexyl, phenyl, biphenyl, naphthyl, anthracene, phenanthrene, thiophene, furanyl, pyrrole, benzothiophene, benzofuranyl, pyridyl, indolyl, cyclopentyl, cyclohexyl, or adamantyl.
3. The organometallic compound according to claim 1 or 2, characterized in that, The structure of the organometallic compound is selected from the group consisting of Formula II - Formula VII:
4. The organometallic compound of claim 3, wherein at least one of R1-R4 is not hydrogen, each independently selected from the group consisting of hydrogen, deuterium, fluorine, cyano, methyl, ethyl, isopropyl, isobutyl, tert-butyl, isopentyl, neopentyl, phenyl, methylphenyl, -CD3, and the following groups; 5. The organometallic compound of claim 3, wherein R9, R 10 R9, R 11 R9, R 12 R9, R 13 R9, R 14 R9, R 15 R9, R 16 are each independently selected from the group consisting of hydrogen, methyl, ethyl, fluoro, cyano, -CD3, t-butyl, i-propyl, n-propyl, and the following groups:
6. The organometallic compound of claim 1, wherein ligand The moiety is selected from the following structures LA-1 to LA-95:
7. The organometallic compound of claim 1, wherein The organometallic compound is selected from one of the following structures:
8. An organic electroluminescent device, characterized by The organic electroluminescent device includes an anode, a cathode, and an organic material layer disposed between the anode and the cathode; the organic material layer contains at least one of the organometallic compounds as described in any one of claims 1-7.
9. The organic electroluminescent device according to claim 8, characterized in that The organic electroluminescent device includes a light-emitting layer, which comprises the aforementioned organometallic compound.
10. The organic electroluminescent device according to claim 9, characterized in that The light-emitting layer of the organic electroluminescent device comprises a host material and a dopant material; the dopant material comprises at least one of the organometallic compounds, and the mass ratio of the host material to the dopant material is (10-99.5):0.5.