Insulating film for solid-state battery, and preparation method therefor and application thereof

By using a modified polyallyl carbonate insulating film in solid-state batteries, the problems of easy breakdown and degraded charge-discharge performance in Hi-pot testing of solid-state batteries have been solved, achieving a high-insulation-performance and easily removable insulating film, thus improving the safety and efficiency of the battery.

WO2026237243A1PCT designated stage Publication Date: 2026-11-19CHERY AUTOMOBILE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2025/124259
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-14
Filing Date
2025-09-26
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Solid-state batteries are prone to breakdown in Hi-pot tests, and the insertion of insulating layers reduces ion conduction efficiency and increases internal resistance, affecting charge and discharge performance.

Method used

Modified polyallyl carbonate insulating films are used by introducing thermosensitive groups, such as tert-butyloxycarbonyl, azodicarbonate, sulfonyl azide, tert-butyl carbonate, or nitro groups, into polyallyl carbonate to prepare insulating films with high electronic impedance and easy decomposition at 120℃-150℃. These films are used between the positive or negative electrode and the solid electrolyte in solid-state batteries.

Benefits of technology

It improves the insulation performance and intrinsic breakdown voltage of solid-state batteries, avoids the risk of breakdown, and makes it easy to remove the insulating film after testing, maintaining charge and discharge performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2025124259_19112026_PF_FP_ABST
    Figure CN2025124259_19112026_PF_FP_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of battery materials, and discloses an insulating film for a solid-state battery, and a preparation method therefor and an application thereof. The insulating film comprises a modified poly(allyl carbonate); the modified poly(allyl carbonate) comprises a thermally sensitive group; the thermally sensitive group is selected from at least one of tert-butoxycarbonyl, azodicarboxylate, sulfonyl azide, tert-butyl carbonate, and nitro; the doping amount of the thermally sensitive group is such that the thermal decomposition temperature of the modified poly(allyl carbonate) is 120°C-150°C. By using the insulating film, the intrinsic breakdown voltage of the solid-state battery can be improved, the risk of the solid-state battery being broken down during high-potential testing can be effectively avoided, and the insulating film can be easily removed after testing, thereby ensuring the quality and charge-discharge performance of the solid-state battery.
Need to check novelty before this filing date? Find Prior Art

Description

Insulating films for solid-state batteries, their preparation methods and applications

[0001] This application claims priority to Chinese Patent Application No. 202510621315.6, filed on May 14, 2025, entitled "Insulating Thin Film for Solid-State Batteries and its Preparation Method and Application", the entire contents of which are incorporated herein by reference. Technical Field

[0002] This application relates to the field of battery materials technology, and in particular to an insulating film for solid-state batteries, its preparation method, and its application. Background Technology

[0003] Hi-pot (High Potential) testing is a test method that tests the insulation performance of a battery by applying a high potential voltage. It can detect defects such as cracks and impurities in the battery and can be used to determine the potential risk of internal short circuit in the battery.

[0004] For solid-state batteries, because their internal solid electrolyte is not completely insulated from electrons, the required test voltage during Hi-pot testing is high, posing a risk of breakdown. Related technologies typically insert an insulating layer into the solid-state battery to increase its intrinsic breakdown voltage and prevent breakdown during Hi-pot testing.

[0005] However, the insertion of the insulating layer reduces the ion conduction efficiency of the solid-state battery, increases its internal resistance, and affects its charge and discharge performance. Summary of the Invention

[0006] This application provides an insulating film for solid-state batteries, its preparation method, and its application, to solve the technical problems existing in related technologies. Specifically, it includes the following technical solutions.

[0007] In a first aspect, this application provides an insulating film for solid-state batteries, the insulating film comprising modified polyallyl carbonate, the modified polyallyl carbonate comprising a thermosensitive group selected from at least one of tert-butyloxycarbonyl, azodicarbonate, sulfonyl azide, tert-butyl carbonate, and nitro, wherein the amount of doping of the thermosensitive group is such that the thermal decomposition temperature of the modified polyallyl carbonate is 120℃-150℃, for example, it can be 120℃, 122℃, 124℃, 126℃, 128℃, 130℃, 132℃, 134℃, 136℃, 138℃, 140℃, 142℃, 144℃, 146℃, 148℃, 150℃, etc., or other values ​​within the above range.

[0008] In some possible embodiments, the doping percentage of the thermosensitive group in the modified polyallyl carbonate is 10%-30%, for example, it can be 10wt%, 11wt%, 12wt%, 13wt%, 14wt%, 15wt%, 16wt%, 17wt%, 18wt%, 19wt%, 20wt%, 21wt%, 22wt%, 23wt%, 24wt%, 25wt%, 26wt%, 27wt%, 28wt%, 29wt%, 30wt%, etc., or other values ​​within the above range.

[0009] In some possible implementations, the electronic impedance of the insulating film is greater than 1.0 × 10⁻⁶. 15 Ω / cm, the electronic impedance of the insulating film can be, for example, 1.1 × 10 Ω / cm. 15 Ω / cm, 1.2×10 15 Ω / cm, 1.3×10 15 Ω / cm, 1.4×10 15 Ω / cm, 1.5×10 15 Ω / cm, 1.6×10 15 Ω / cm, 1.7×10 15 Ω / cm, 1.8×10 15 Ω / cm, 1.9×10 15 Ω / cm, 2.0×10 15 Ω / cm, 2.1×10 15 Ω / cm, 2.2×10 15 Ω / cm, 2.3×10 15 Ω / cm, 2.4×10 15 Ω / cm, 2.5×10 15 Ω / cm, 2.6×10 15 Ω / cm, 2.7×10 15 Ω / cm, or other values ​​within the above range, are not limited in this application.

[0010] In some possible implementations, the thickness of the insulating film is 5 μm-30 μm.

[0011] Secondly, this application provides a method for preparing an insulating film, the method comprising: preparing modified polyallyl carbonate, wherein the modified polyallyl carbonate includes a thermosensitive group, the thermosensitive group being selected from at least one of tert-butyloxycarbonyl, azodicarbonate, sulfonyl azide, tert-butyl carbonate, and nitro, wherein the doping amount of the thermosensitive group is such that the thermal decomposition temperature of the modified polyallyl carbonate is 120℃-150℃; and preparing the insulating film by a thin-film forming process from the modified polyallyl carbonate.

[0012] Thirdly, this application provides a solid-state battery, the solid-state battery comprising a positive electrode, a negative electrode, a solid electrolyte, and an insulating film as described in any one of the first aspects of this application; the insulating film is located between at least one of the positive electrode and the negative electrode and the solid electrolyte.

[0013] In some possible implementations, the insulating film is located between the positive electrode and the solid electrolyte.

[0014] In some possible implementations, the insulating film is located between the negative electrode and the solid electrolyte.

[0015] Fourthly, this application provides a method for testing the insulation performance of a solid-state battery, the method comprising: testing the solid-state battery through a high-potential testing process, wherein the solid-state battery is a solid-state battery as described in any one of the first aspects of this application; and performing heat preservation treatment on the tested solid-state battery at 120℃-150℃.

[0016] In some possible implementations, the heat preservation treatment lasts for 30-60 minutes.

[0017] The beneficial effects of the technical solution provided in this application include at least the following:

[0018] The insulating film for solid-state batteries provided in this application, by introducing specific thermosensitive groups into polyallyl carbonate, retains the excellent electronic insulation properties of polyallyl carbonate while exhibiting poor thermal stability due to the introduced thermosensitive groups, making it prone to decomposition at 120°C-150°C. Specifically, the embodiments of this application select specific thermosensitive groups to ensure that the insulating film leaves no moisture or other solid residues after thermal decomposition. When applied to solid-state batteries, particularly in high-potential testing, this insulating film can improve the intrinsic breakdown voltage of the solid-state battery, effectively avoiding the risk of breakdown, and facilitating the removal of the insulating film after testing, thus improving the charge-discharge performance of the solid-state battery. Attached Figure Description

[0019] To more clearly illustrate the technical solutions in the embodiments of this application, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0020] Figure 1 is a schematic diagram of the solid-state battery provided in an embodiment of this application;

[0021] Figure 2 is a schematic diagram of another solid-state battery provided in an embodiment of this application. Detailed Implementation

[0022] An internal short circuit in a solid-state battery refers to an undesirable direct or indirect connection between the positive and negative electrodes within the battery, causing current to bypass the normal operating circuit and flow directly through the short circuit point. For example, defects, cracks, voids, or impurities in the solid electrolyte within the battery can create abnormal electron conduction paths, leading to a short circuit within the battery.

[0023] Internal short circuits severely impact the electrical performance of solid-state batteries and increase the risk of thermal runaway. Therefore, to mitigate the effects of internal short circuits on solid-state batteries, an insulating layer can be inserted, allowing for high-potential testing to detect internal short circuits. However, the insertion of the insulating layer also reduces the ion conduction efficiency and increases the internal resistance of the solid-state battery, thus affecting its charge-discharge performance.

[0024] To address the technical problem that inserting an insulating layer into a solid-state battery to improve its insulation performance can negatively impact its charge-discharge performance, this application provides an insulating film for solid-state batteries. This film not only improves the insulation performance of the solid-state battery but also allows for thermal decomposition to remove impurities as needed for specific applications, thus ensuring the battery's charge-discharge performance. Specifically, the products of the thermal decomposition of this insulating film are free of moisture and solid residues.

[0025] The first aspect of this application discloses an insulating film for solid-state batteries. The insulating film includes modified polyallyl carbonate, which includes a thermosensitive group selected from at least one of tert-butyloxycarbonyl, azodicarbonate, sulfonyl azide, tert-butyl carbonate, and nitro. The amount of thermosensitive group doped is such that the thermal decomposition temperature of the modified polyallyl carbonate is 120°C-150°C.

[0026] It should be noted that the modified polyallyl carbonate involved in the embodiments of this application refers to polyallyl carbonate modified with thermosensitive groups, which includes polyallyl carbonate and thermosensitive groups grafted onto the polyallyl carbonate. The terminal hydroxyl groups of the polyallyl carbonate serve as reaction sites, reacting with the thermosensitive groups, thereby modifying the polyallyl carbonate to be thermosensitive group-terminated polyallyl carbonate.

[0027] The polyallyl carbonate involved in the embodiments of this application, also known as polypropylene carbonate, has the following chemical structural formula.

[0028] In some examples, the relative molecular weight of polyallyl carbonate applicable to the embodiments of this application can be 5000 g / mol to 20000 g / mol.

[0029] Polyallyl carbonate can be used, but is not limited to, to provide good insulation properties for modified polyallyl carbonate and insulating films, so that when the insulating film is used in solid-state batteries, it can effectively improve the internal insulation performance of solid-state batteries, thereby increasing the intrinsic breakdown voltage of solid-state batteries (i.e., the maximum electric field strength or voltage value that solid-state batteries can withstand without the influence of external defects or other non-ideal factors), so as to avoid the solid-state batteries being broken down in high-potential tests with high test voltages.

[0030] Thermosensitive groups can be used, but are not limited to, to improve the thermosensitivity of modified polyallyl carbonate and insulating films, making the insulating films easily decomposed by heat. This allows the insulating films to be removed as needed for actual applications when used in solid-state batteries, thus ensuring the charge and discharge performance of the solid-state batteries.

[0031] Optionally, the thermosensitive group may be selected from at least one of tert-butyloxycarbonyl, azodicarbonate, sulfonyl azide, tert-butyl carbonate, and nitro, so that the insulating film leaves no moisture or solid residue after thermal decomposition. For example, when the thermosensitive group is tert-butyloxycarbonyl, the carbonate bonds in the modified polyallyl carbonate break after heating, generating carbon dioxide and allyl ether gases; when the thermosensitive group is azodicarbonate, the carbonate bonds in the modified polyallyl carbonate break after heating, generating carbon dioxide and allyl ether gases; when the thermosensitive group is sulfonyl azide, the decomposition products of the insulating film after heating are nitrogen and sulfur dioxide; when the thermosensitive group is tert-butyl carbonate, the decomposition products of the insulating film after heating are carbon dioxide and isobutylene; when the thermosensitive group is nitro, the decomposition products of the insulating film after heating are nitrogen dioxide and nitric oxide.

[0032] In some embodiments, the amount of thermosensitive group doped in the modified polyallyl carbonate makes the thermal decomposition temperature of the modified polyallyl carbonate 120℃-150℃, for example, it can be 120℃, 122℃, 124℃, 126℃, 128℃, 130℃, 132℃, 134℃, 136℃, 138℃, 140℃, 142℃, 144℃, 146℃, 148℃, 150℃, etc., or other values ​​within the above range.

[0033] In some embodiments, the mass percentage of the thermosensitive group in the modified polyallyl carbonate is 10wt%-30wt%, for example, it can be 10wt%, 11wt%, 12wt%, 13wt%, 14wt%, 15wt%, 16wt%, 17wt%, 18wt%, 19wt%, 20wt%, 21wt%, 22wt%, 23wt%, 24wt%, 25wt%, 26wt%, 27wt%, 28wt%, 29wt%, 30wt%, etc., or other values ​​within the above range.

[0034] For example, in order for solid-state batteries to exhibit good insulation properties, the electronic impedance of the insulating film is greater than 1.0 × 10⁻⁶. 15 Ω / cm, the electronic impedance of the insulating film can be, for example, 1.1 × 10 Ω / cm. 15 Ω / cm, 1.2×10 15 Ω / cm, 1.3×10 15 Ω / cm, 1.4×10 15 Ω / cm, 1.5×10 15 Ω / cm, 1.6×10 15 Ω / cm, 1.7×10 15 Ω / cm, 1.8×10 15 Ω / cm, 1.9×10 15 Ω / cm, 2.0×10 15 Ω / cm, 2.1×10 15 Ω / cm, 2.2×10 15 Ω / cm, 2.3×10 15 Ω / cm, 2.4×10 15 Ω / cm, 2.5×10 15 Ω / cm, 2.6×10 15 Ω / cm, 2.7×10 15 Ω / cm, or other values ​​within the above range, are not limited in this application.

[0035] In some embodiments, to avoid affecting the charge and discharge performance of the solid-state battery, the thickness of the insulating film is 5μm-30μm.

[0036] The insulating film for solid-state batteries provided in this application, by introducing specific thermosensitive groups into polyallyl carbonate, retains the excellent electronic insulation properties of polyallyl carbonate while exhibiting poor thermal stability due to the introduced thermosensitive groups, making it prone to decomposition at 120°C-150°C. Specifically, the embodiments of this application select specific thermosensitive groups to ensure that the insulating film leaves no moisture or other solid residues after thermal decomposition. When applied to solid-state batteries, particularly in high-potential testing, this insulating film can improve the intrinsic breakdown voltage of the solid-state battery, effectively avoiding the risk of breakdown, and facilitating the removal of the insulating film after testing, thus improving the charge-discharge performance of the solid-state battery.

[0037] In some examples, the insulating film for solid-state batteries mentioned above can be prepared by the following methods.

[0038] Step 1: Preparation of modified polyallyl carbonate.

[0039] The modified polyallyl carbonate includes a thermosensitive group, which is selected from at least one of tert-butyloxycarbonyl, azodicarbonate, sulfonyl azide, tert-butyl carbonate, and nitro. The amount of thermosensitive group doping results in a thermal decomposition temperature of 120℃-150℃ for the modified polyallyl carbonate, such as 120℃, 122℃, 124℃, 126℃, 128℃, 130℃, 132℃, 134℃, 136℃, 138℃, 140℃, 142℃, 144℃, 146℃, 148℃, 150℃, or other values ​​within the above range.

[0040] For example, modified polyallyl carbonate is prepared by the following method:

[0041] Under light-protected conditions, allyl carbonate and a thermosensitive compound containing thermosensitive groups are dissolved in a solvent, and the reaction is carried out with triethylamine as an initiator to obtain modified allyl carbonate. The thermosensitive compound contains the thermosensitive groups mentioned above.

[0042] For example, when the thermosensitive group is tert-butoxycarbonyl, the corresponding thermosensitive compound can be tert-butoxycarbonyl anhydride. When the thermosensitive group is azodicarbonate, the corresponding thermosensitive compound can be azodicarbonyl chloride. When the thermosensitive group is sulfonyl azide, the corresponding thermosensitive compound can include sulfonyl chloride and sodium azide. When the thermosensitive group is tert-butyl carbonate, the corresponding thermosensitive compound can include tert-butyl chloroformate and pyridine.

[0043] Step 2: Prepare an insulating film from modified polyallyl carbonate using a thin-film process.

[0044] In some embodiments, the thin-film process includes, for example, a casting process, and the method for preparing an insulating film from modified polyallyl carbonate by the thin-film process includes, for example, preparing an insulating film from modified polyallyl carbonate by the casting process.

[0045] It should be noted that the method for preparing the insulating film provided in the above embodiments is based on the same concept as the insulating film embodiment for solid-state batteries. For detailed description of the insulating film, please refer to the insulating film embodiment for solid-state batteries. The same content will not be repeated here.

[0046] This application also provides a solid-state battery, which includes a positive electrode, a negative electrode, a solid electrolyte, and an insulating film as described above, wherein the insulating film is located between at least one of the positive electrode and the negative electrode and the solid electrolyte.

[0047] Optionally, the insulating film may be located between the positive electrode and the solid electrolyte, such that the insulating film forms an insulating layer between the positive electrode and the solid electrolyte of the solid battery to block the electronic conduction path inside the solid battery; or the insulating film may be located between the negative electrode and the solid electrolyte, such that the insulating film forms an insulating layer between the negative electrode and the solid electrolyte of the solid battery to block the electronic conduction path inside the solid battery.

[0048] In some embodiments, the solid-state battery provided in this application may further include a positive current collector disposed on the side of the positive electrode away from the solid electrolyte, and a negative current collector disposed on the side of the negative electrode away from the solid electrolyte.

[0049] Figure 1 is a schematic diagram of the structure of a solid-state battery provided in an embodiment of this application. Referring to Figure 1, the solid-state battery provided in an embodiment of this application includes, for example, a positive current collector 110, a positive electrode 120, an insulating film 130, a solid electrolyte 140, a negative electrode 150, and a negative current collector 160 stacked sequentially.

[0050] The positive current collector 110 can be used, but is not limited to, to collect the current generated by the positive electrode and conduct it to an external circuit. The positive current collector may include, for example, aluminum foil. The positive electrode 120 can be used, but is not limited to, to store or release electrical energy through the insertion / extraction of metal ions (e.g., lithium ions or other metal ions). An insulating film 130 is disposed between the positive electrode 120 and the solid electrolyte 140, and can be used, but is not limited to, to improve the insulation performance of the solid-state battery. The solid electrolyte 140 can be used, but is not limited to, to conduct metal ions (e.g., lithium ions or other metal ions). The negative electrode 150 can be used, but is not limited to, to store or release electrical energy through the insertion / extraction of metal ions (e.g., lithium ions or other metal ions).

[0051] Figure 2 is a schematic diagram of another solid-state battery provided in an embodiment of this application. Referring to Figure 2, another solid-state battery provided in an embodiment of this application includes, for example, a positive current collector 210, a positive electrode 220, a solid electrolyte 230, an insulating film 240, a negative electrode 250, and a negative current collector 260 stacked sequentially.

[0052] It should be noted that the solid-state battery shown in Figure 2 differs from the solid-state battery shown in Figure 1 in that the insulating film 240 is disposed between the negative electrode 250 and the solid electrolyte 230. The same content will not be repeated here.

[0053] The solid-state battery provided in this application includes an insulating film. By introducing specific thermistor groups into the insulating film, the solid-state battery exhibits excellent insulation properties, which helps improve its intrinsic breakdown voltage. This allows for testing of the internal short-circuit condition of the solid-state battery through high-potential testing. Furthermore, the insulating film readily decomposes at 120℃-150℃, and the decomposition products contain no moisture or solid residue, thus ensuring the charge-discharge performance of the solid-state battery. In addition, the solid-state battery provided in this application allows for adjustment of the insulating film's position according to the needs of specific application scenarios to adapt to different manufacturing processes, thereby reducing the manufacturing difficulty of the solid-state battery.

[0054] This application also provides a method for testing the insulation performance of solid-state batteries, the method comprising the following steps.

[0055] Step 1: The solid-state battery is tested using a high-potential testing process, wherein the solid-state battery used is the one described above.

[0056] Step 2: Perform heat preservation treatment on the tested solid-state battery at 120℃-150℃.

[0057] In some embodiments, the heat preservation treatment lasts for 30-60 minutes.

[0058] The solid-state battery insulation performance testing method provided in this application includes an insulating film. By introducing specific thermosensitive groups into the insulating film, on the one hand, the solid-state battery has a higher intrinsic breakdown voltage, which is beneficial to improving the reliability of the test results when testing the internal short circuit of the solid-state battery through high-potential testing. On the other hand, after the high-potential test, the insulating film can be removed by heat preservation treatment of the solid-state battery at 120℃-150℃, which is beneficial to improving the charge and discharge performance of the solid-state battery.

[0059] Exemplary embodiments of the present invention will now be described in more detail. While exemplary embodiments of the present invention are described below, it should be understood that the present invention can be implemented in various forms and should not be limited to the embodiments set forth herein. Where specific techniques or conditions are not specified in the embodiments, they are performed in accordance with techniques or conditions described in the literature in the art or according to product instructions. Reagents or instruments used, unless otherwise specified, are all commercially available conventional products.

[0060] In all the following examples, "10.0 g of allyl carbonate (0.8 mmol repeating unit)" refers to the total amount of repeating molecular chain units in a 10.0 g polypropylene carbonate sample being 0.8 mmol. Correspondingly, the relative molecular mass M of this allyl carbonate is calculated using the following formula: M = 10.0 g / 8 × 10⁻⁶ -4 mol = 12500 g / mol.

[0061] Example 1

[0062] Example 1 provides a method for preparing an insulating film, comprising the following steps:

[0063] Step 1: Preparation of modified polyallyl carbonate with tert-butyloxycarbonyl groups, which includes:

[0064] 10.0 g of polyallyl carbonate (0.8 mmol repeating unit) was dissolved in 150 ml of anhydrous dichloromethane, and then 18.5 g of tert-butyloxycarbonyl anhydride (85 mmol) and 0.5 g of 4-dimethylaminopyridine were added. The mixture was stirred and reacted at 55 °C under a nitrogen atmosphere for 24 h. Cold methanol was then added to the product, and the resulting precipitate was dried under vacuum to obtain a white powder, which is tert-butyloxycarbonyl modified polyallyl carbonate.

[0065] Step 2: An insulating film is prepared from tert-butyloxycarbonyl modified polyallyl carbonate using a casting process. This includes: uniformly casting the tert-butyloxycarbonyl modified polyallyl carbonate onto a substrate using a casting machine to form a uniform wet film; and drying the wet film to obtain the insulating film. The thickness of the insulating film is 10 μm.

[0066] The resistance of the insulating film prepared in Example 1 was tested using AC impedance spectroscopy. The test steps included: sandwiching the insulating film between two stainless steel sheets to assemble it into a coin cell, and then using an electrochemical workstation to test the impedance response of the insulating film in the frequency range of 0.1 Hz to 1 MHz. The electronic impedance of the insulating film was obtained by fitting a series resistance model. The test results are shown in Table 1.

[0067] Example 2

[0068] Example 2 provides a method for preparing an insulating film, comprising the following steps:

[0069] Step 1: Preparation of modified polyallyl carbonate incorporating azodicarbonate, which includes:

[0070] Under light-protected conditions, 10.0 g of polyallyl carbonate (0.8 mmol repeating unit) and 12.3 g of azodicarbonyl chloride (75 mmol) were dissolved in 120 ml of anhydrous THF (Tetrahydrofuran), and then 15 ml of triethylamine was added. The mixture was reacted at 0 °C for 6 h, and then the temperature was raised to 25 °C and the reaction was continued for 12 h. The product was extracted with diethyl ether / water, and the resulting orange solid was purified to obtain azodicarbonyl ester modified polyallyl carbonate.

[0071] Step 2: Prepare an insulating film from azodicarbonate-modified allyl carbonate using a casting process, which includes:

[0072] Tert-butyloxycarbonyl modified polyallyl carbonate is uniformly cast onto a substrate using a casting machine to form a uniform wet film. After drying, the wet film yields an insulating film with a thickness of 10 μm.

[0073] The resistance of the insulating film prepared in Example 2 was tested using AC impedance spectroscopy. The test steps included: sandwiching the insulating film between two stainless steel sheets to assemble it into a coin cell, and then using an electrochemical workstation to test the impedance response of the insulating film in the frequency range of 0.1 Hz to 1 MHz. The electronic impedance of the insulating film was obtained by fitting a series resistance model. The test results are shown in Table 1.

[0074] Example 3

[0075] Example 3 provides a method for preparing an insulating film, comprising the following steps:

[0076] Step 1: Preparation of modified polyallyl carbonate incorporating sulfonyl azide, which includes:

[0077] At 80°C, 10.0 g of polyallyl carbonate (0.8 mmol repeating unit) and 9.5 g of sulfonyl chloride (70 mmol) were reacted in toluene for 5 h to generate a sulfonyl chloride intermediate. After cooling to 0°C, a DMF (Dimethylformamide, N,N-dimethylformamide) solution of sodium azide (6.8 g of sodium azide and 105 mmol of molar amount) was added. The mixture was then stirred at room temperature for 8 h. After dialysis purification, a pale yellow product was obtained, which is sulfonyl azide-modified polyallyl carbonate.

[0078] Step 2: Prepare an insulating film from sulfonyl azide-modified allyl carbonate using a casting process, which includes:

[0079] Tert-butyloxycarbonyl modified polyallyl carbonate is uniformly cast onto a substrate using a casting machine to form a uniform wet film. After drying, the wet film yields an insulating film with a thickness of 10 μm.

[0080] The resistance of the insulating film prepared in Example 3 was tested using AC impedance spectroscopy. The test steps included: sandwiching the insulating film between two stainless steel sheets to assemble it into a coin cell, and then using an electrochemical workstation to test the impedance response of the insulating film in the frequency range of 0.1 Hz to 1 MHz. The electronic impedance of the insulating film was obtained by fitting a series resistance model. The test results are shown in Table 1.

[0081] Example 4

[0082] Example 4 provides a method for preparing an insulating film, comprising the following steps:

[0083] Step 1: Preparation of modified polyallyl carbonate incorporating tert-butyl carbonate, which includes:

[0084] 10.0 g of polyallyl carbonate (0.8 mmol repeat unit) 、 13.2 g of tert-butyl chloroformate (90 mmol) and 7.1 ml of pyridine were dissolved in 120 ml of toluene solution and reacted at 45 °C for 36 h. Then, n-hexane was added to the reaction product to obtain a transparent elastomer, which is tert-butyl carbonate modified polyallyl carbonate.

[0085] Step 2: An insulating film is prepared from modified polyallyl carbonate incorporating tert-butyl carbonate using a casting process. This includes:

[0086] Tert-butyloxycarbonyl modified polyallyl carbonate is uniformly cast onto a substrate using a casting machine to form a uniform wet film. After drying, the wet film yields an insulating film with a thickness of 10 μm.

[0087] The resistance of the insulating film prepared in Example 4 was tested using AC impedance spectroscopy. The test steps included: sandwiching the insulating film between two stainless steel sheets to assemble it into a coin cell, and then using an electrochemical workstation to test the impedance response of the insulating film in the frequency range of 0.1 Hz to 1 MHz. The electronic impedance of the insulating film was obtained by fitting a series resistance model. The test results are shown in Table 1.

[0088] Table 1

[0089] As shown in Table 1, the insulating films provided in this application have high electronic impedance and good electronic insulation performance, which can greatly improve the insulation performance inside the solid-state battery, effectively block the electronic conduction path inside the solid-state battery, and make the solid-state battery in an open circuit state.

[0090] When this insulating film is applied to solid-state batteries, it effectively avoids the risk of internal breakdown during high-potential testing to assess internal short-circuit conditions. This improves the internal insulation performance of the solid-state battery and ensures its quality. Specifically, the insulating film decomposes into gas at 120°C-150°C, facilitating its removal after testing and ensuring the battery's charge-discharge performance.

[0091] The above description is only for the purpose of enabling those skilled in the art to understand the technical solution of this application, and is not intended to limit this application. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the protection scope of this application.

Claims

1. An insulating film for a solid state battery, wherein, The insulating film comprises modified polyallyl carbonate, the modified polyallyl carbonate comprising a thermosensitive group selected from at least one of tert-butyloxycarbonyl, azodicarbonate, sulfonyl azide, tert-butyl carbonate and nitro, the amount of thermosensitive group doped such that the thermal decomposition temperature of the modified polyallyl carbonate is 120℃-150℃.

2. The insulating film according to claim 1, wherein, The percentage of the thermosensitive group in the modified polyallyl carbonate is 10%-30%.

3. The insulating film of claim 1, wherein, The electronic impedance of the insulating film is greater than 1.0 x 10 15 Ω / cm.

4. The insulating film of claim 1, wherein, The thickness of the insulating film is 5μm-30μm.

5. A method of making an insulating film, wherein, The method includes: A modified polyallyl carbonate is prepared, wherein the modified polyallyl carbonate includes a thermosensitive group, the thermosensitive group being selected from at least one of tert-butyloxycarbonyl, azodicarbonate, sulfonyl azide, tert-butyl carbonate and nitro, and the doping amount of the thermosensitive group is such that the thermal decomposition temperature of the modified polyallyl carbonate is 120℃-150℃. The insulating film is prepared by the modified polyallyl carbonate through a thin-film process.

6. A solid-state battery, wherein, The solid-state battery includes a positive electrode, a negative electrode, a solid electrolyte, and an insulating film as described in any one of claims 1-4; The insulating film is located between at least one of the positive electrode and the negative electrode and the solid electrolyte.

7. The solid-state battery of claim 6, wherein, The insulating film is located between the positive electrode and the solid electrolyte.

8. The solid-state battery of claim 6, wherein, The insulating film is located between the negative electrode and the solid electrolyte.

9. A method of testing the insulation properties of a solid state battery, wherein, The method includes: The solid-state battery is tested using a high-potential testing process, wherein the solid-state battery is the solid-state battery as described in any one of claims 6-8; The solid-state battery was subjected to heat preservation treatment at 120℃-150℃ after testing.

10. The method of claim 9, wherein, The heat preservation treatment lasts for 30-60 minutes.