Preparation method for and use of low-temperature-resistant high-purity perfluoroether rubber

By initiating polymerization in a microemulsion system, a low-temperature resistant, high-purity perfluoroether rubber was prepared, solving the problem of low product purity in existing technologies. This resulted in a perfluoroether rubber with high mechanical properties and low-temperature resistance, suitable for cutting-edge products.

WO2026237262A1PCT designated stage Publication Date: 2026-11-19ZHEJIANG JUSHENG FLUOROCHEM
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2025/128584
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-14
Filing Date
2025-10-17
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing technologies make it difficult to synthesize low-temperature resistant, high-purity perfluoroether rubber in microemulsion systems, and the product purity is not high, making it difficult to apply to cutting-edge products such as electronic chips.

Method used

Comonomers A and B, tetrafluoroethylene and perfluoroalkyl vinyl ethers were used as reactants to initiate a polymerization reaction under microemulsion conditions. Iodinated fluoroolefins were added as vulcanization point monomers and iodinated alkanes as chain transfer agents. Perfluoroether rubber was prepared by controlling the pressure and temperature of the polymerization reactor. Triallylsilsesquioxane was used as a modified vulcanizing agent to improve the crosslinking density.

Benefits of technology

The prepared perfluoroether rubber has excellent mechanical properties, low-temperature resistance and chemical stability, with a tensile strength ≥26MPa, elongation at break ≥250%, and a minimum low-temperature resistance of -50℃, making it suitable for high-end products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2025128584-FTAPPB-I100001
    Figure PCTCN2025128584-FTAPPB-I100001
  • Figure PCTCN2025128584-FTAPPB-I100002
    Figure PCTCN2025128584-FTAPPB-I100002
  • Figure PCTCN2025128584-FTAPPB-I100003
    Figure PCTCN2025128584-FTAPPB-I100003
Patent Text Reader

Abstract

The present disclosure relates to the technical field of fluoroether rubber, and discloses a preparation method for and the use of low-temperature-resistant high-purity perfluoroether rubber. The preparation method comprises the following specific steps: adding high-purity water, a microemulsion, a monomer A and a monomer B to a polymerization kettle, starting stirring, heating the polymerization kettle while introducing PMVE, then introducing a first mixed gas of PMVE and TFE, a chain transfer agent, a cure-site monomer and an initiator, introducing a second mixed gas of PMVE and TFE during the reaction process, releasing the pressure of the polymerization kettle after a copolymerization reaction is terminated, then performing discharging to obtain an elastomer emulsion, condensing, washing and drying same to obtain perfluoroether rubber, and performing mixing to finally obtain vulcanized perfluoroether rubber. A perfluoromethyl vinyl ether-tetrafluoroethylene copolymer prepared in the present disclosure has good mechanical properties, low-temperature resistance and vulcanization properties.
Need to check novelty before this filing date? Find Prior Art

Description

A method for preparing and applying low-temperature resistant high-purity perfluoroether rubber

[0001] Cross-reference to related applications

[0002] This disclosure is based on and claims priority to Chinese Patent Application No. 202510616180.4, filed on May 14, 2025, the entire contents of which are incorporated herein by reference. Technical Field

[0003] This disclosure relates to the field of fluoroether rubber technology, and in particular to a method for preparing and applying low-temperature resistant high-purity perfluoroether rubber. Background Technology

[0004] Perfluoroelastomers are widely used in the sealing of chemical reaction equipment in various factories, chemical pipeline linings and fittings, semiconductor industry seals, and special parts in the automotive, petrochemical and aerospace industries.

[0005] Patent document CN105218985 discloses a method for improving the corrosion resistance of fluororubber, particularly its resistance to hydrofluoric acid. The specific method involves adding a certain amount of perfluoroether rubber to fluororubber. While this method improves the corrosion resistance of fluororubber, the blended material significantly reduces the excellent resistance of the perfluoroether rubber to various media. This patent does not investigate the low-temperature performance of the perfluoroether rubber.

[0006] Patent document CN110903428 A discloses a low-temperature resistant fluoroether rubber, its preparation method, and its application. It is obtained by emulsion polymerization of one or more comonomers of vinylidene fluoride / tetrafluoroethylene / perfluoropropylene, low-temperature comonomer perfluoroalkyl vinyl ether, vulcanizing point monomer iodoperfluoroolefin, and chain transfer agent iodoalkane under certain temperature and pressure. However, the permanent compression set (O-ring, 200℃, 70h) of the obtained rubber product is more than 20%, the glass transition temperature is between -22℃ and -37℃, and the tensile strength is about 18MPa-25MPa.

[0007] Patent document CN104530292A discloses a method for preparing low-temperature resistant perfluoroether rubber. The method involves mixing emulsifier, fluoroether oil, and water in a specific ratio and heating to form a microemulsion. Then, comonomer A, comonomer B, tetrafluoroethylene, perfluoromethyl vinyl ether, a pH adjuster, and an initiator are added to react. Perfluoroether rubber prepared using this method is easy to process, with a glass transition temperature of -29 to -36°C, a tensile strength of approximately 18 to 23 MPa, and an elongation at break of 220 to 250. However, if the copolymerization temperature is below 70°C, the polymerization rate is too slow for industrial production. If the temperature is above 120°C, the fluorinated elastomer polymer emulsion becomes viscous and clogs the pipes, making it difficult to maintain the stability of the emulsion during the reaction, resulting in poor experimental repeatability.

[0008] While the perfluoroether rubber produced by the existing PMVE-TFE process exhibits some low-temperature resistance, its low purity makes it difficult to apply to advanced products such as electronic chips. There is an urgent need to find a method for synthesizing low-temperature resistant, high-purity perfluoroether rubber using a microemulsion system. Although methods for synthesizing low-temperature fluoroether rubber using microemulsion systems have been reported, the preparation of the microemulsion in these methods is highly temperature-dependent, requiring preheating before the reaction, and the microemulsion system is unstable and prone to stratification. Furthermore, the purity of the produced product is low, failing to meet the requirements of advanced electronic products. Summary of the Invention

[0009] This disclosure provides a method for preparing and applying a low-temperature resistant, high-purity perfluoroether rubber. The rubber is obtained by polymerization under microemulsion conditions using comonomers A and B as comonomers, tetrafluoroethylene and perfluoroalkyl vinyl ether as reactants, iodofluoroolefins as vulcanizing point monomers, and iodoalkanes as chain transfer agents.

[0010] The specific plan is as follows:

[0011] A method for preparing and applying low-temperature resistant high-purity perfluoroether rubber, the operation steps of which are as follows:

[0012] S1: According to the weight percentage, add 300-400 parts of high-purity water to the polymerization reactor, start stirring and add 0.5-2 parts of microemulsion, add 0.25-0.45 parts of comonomers A and B to the microemulsion, stir at 30-120 rpm, heat the polymerization reactor while introducing PMVE, until the temperature reaches 80-120℃ and the pressure reaches 1.5-1.8 MPa, then introduce the first mixed gas of PMVE and TFE until the pressure in the polymerization reactor reaches 3.0-5.0 MPa, add 0.05-0.2 parts of chain transfer agent, 0.02-0.1 parts of sulfurization point monomer, and 0.01-0.1 parts of initiator to initiate the copolymerization reaction;

[0013] S2: After the polymerization reaction begins, a second mixed gas of PMVE and TFE is introduced to maintain the pressure of the polymerization reactor at 3.0-5.0 MPa and the temperature at 80-120℃. When the consumption of the second mixed monomer reaches 30-50 parts, the copolymerization reaction is terminated, the polymerization reactor is depressurized and discharged, and the obtained elastomer emulsion is coagulated, washed and dried to obtain perfluoroether rubber.

[0014] S3: The following compounding components are prepared: (1) 10-12 parts raw rubber; (2) 0.15-0.18 parts triallyl silsesquioxane modified vulcanizing agent; (3) 0.3-0.5 parts vulcanizing aid 2,5-di-tert-butylperoxide-2,5-dimethylethane; (4) 1.5-2 parts filler material MT carbon black N9900; (5) 0.5-0.8 parts processing aid octadecanoic acid. The above components are added to a mixer and mixed. After being placed at room temperature for 20 hours, the mixture is re-milled on a two-roll mill to finally obtain perfluoroether rubber vulcanizate.

[0015] The mass ratio of the microemulsion is emulsifier:polyether oil:water = 10:1 to 1:10 to 1:10.

[0016] The emulsifier is selected from potassium perfluoropolyether carboxylate, magnesium perfluoropolyether carboxylate, sodium perfluoropolyether carboxylate, and ammonium perfluoropolyether carboxylate; the polyether oil is selected from PFPE, with the structural formula (—CF2—O—CF2—)n.

[0017] The comonomer A is selected from CF3CF2CF2CF2O(CF(CF3)CF2O)nCF=CF2, n=0-6, and can be selected from n=1-3; the comonomer B is selected from CF3CF2O(CF3CF2O)mCF=CF2, m=0-5, and can be selected from m=1-3.

[0018] The chain transfer agent is selected from iodoalkanes, alkane compounds, alcohols, esters, and organohalides, including one or more combinations of 1,3-diiodoperfluoropropane, 1,4-diiodoperfluorobutane, 1,3-diiodo-2-chloroperfluoropropane, 1,5-diiodo-2,4-dichloroperfluoropentane, 1,3-diiodoperfluorobutane, 1,6-diiodoperfluorohexane, 1,8-diiodoperfluorooctane, perfluoroisopropyl iodine, perfluoron-butyl iodine, trifluoromethyl iodine, methyl iodine, isopentane, methanol, isopropanol, ethyl acetate, diethyl malonate, CCl4, CBrCl3, CF2BrCFBrCF3, and CF2I2.

[0019] The sulfidation point monomer is selected from chlorinated alkenes, including one or more combinations of trifluoroethylene bromide, 4-bromoperfluoro-1-butene, 1-bromo-2,2-difluoroethylene, 4-bromo-3,3,4,4-tetrafluoro-1-butene, perfluoroalkyl bromide, 4-bromo-1,1,2-trifluoro-1-butene, and 4-bromo-1,1,3,3,4,4-hexafluoro-1-butene.

[0020] The initiator is selected from one or a combination of several of the following: diisopropyl peroxide, benzoyl peroxide, isopropylbenzene peroxide, tert-butyl hydroperoxide, potassium persulfate, and ammonium persulfate.

[0021] The molar ratio of PMVE to TFE in the first mixed gas is 1:1.0-2.0; the molar ratio of PMVE to TFE in the second mixed gas is 1:1.5-2.0; and the purity of the PMVE and TFE monomers is not less than 99.99%.

[0022] The triallyl silsesquioxane modified vulcanizing agent undergoes a condensation reaction between isocyanurate and hydroxyl groups. In this process, the carbon-nitrogen double bond (C=N) in TAIC reacts with the hydroxyl group (-OH) of the 4,4'-dihydroxy-2,2'-bipyridine / zirconium / lanthanum complex. Through a nucleophilic addition mechanism, the oxygen atom on the hydroxyl group attacks the carbon atom on the TAIC ring, opening the ring to form an intermediate, which is then deprotonated and closed to form a stable urea ketone structure.

[0023] The role of silsesquioxanes: Trisilyl phenyl-cage polysilsesquioxanes may act as templates or scaffolds in this process. Their porous structure and high specific surface area provide a good reaction interface between TAIC and the complex, and promote the reaction through physical adsorption or chemical bonding.

[0024] The preparation method of triallylsilsesquioxane modified vulcanizing agent is as follows:

[0025] By weight, add 25-50 parts of triallyl isocyanurate (TAIC, CAS: 1025-16-2), 0.5-2.5 parts of 4,4'-dihydroxy-2,2'-bipyridine / zirconium / lanthanum complex, 0.01-0.1 parts of trisilyl phenyl-cage polysilsesquioxane (CAS: 444315-26-8), 1-3 parts of stannous octoate, and 200-300 parts of toluene to a sealed stirred reactor. Stir at 60-70°C for 120-180 minutes, and remove the toluene by distillation to obtain the triallyl silsesquioxane modified vulcanizing agent.

[0026] The preparation method of the 4,4'-dihydroxy-2,2'-bipyridine / zirconium / lanthanum complex is as follows: 16-32 parts of 4,4'-dihydroxy-2,2'-bipyridine, 7-14 parts of zirconium nitrate, 16-32 parts of lanthanum nitrate, 200-300 parts of water, stirred at 40-50℃ for 100-150 minutes, and the water was removed by distillation to obtain the 4,4'-dihydroxy-2,2'-bipyridine / zirconium / lanthanum complex.

[0027] The technical effects of this method are as follows:

[0028] (1) Improvement of physical properties: The vulcanization efficiency of fluororubber is improved by introducing 4,4'-dihydroxy-2,2'-bipyridine / zirconium / lanthanum complex and sesquioxane, because these two compounds provide more crosslinking points, which increases the crosslinking density during the vulcanization process, thereby improving the hardness and tear resistance of the material.

[0029] (2) Improved heat resistance: TAIC itself has good thermal stability, and the cross-linked structure formed during its vulcanization process can further improve the heat resistance of the material. At the same time, the silicon-oxygen-silicon bonds of silsesquioxane also have good thermal stability, and their addition helps to improve the overall heat resistance of the material.

[0030] (3) Enhanced chemical stability: The urea ketone structure formed by the above chemical reaction is relatively stable and is not prone to reverse reaction or decomposition under changes in the external environment, thereby enhancing the chemical stability of the material.

[0031] (4) The perfluoromethyl vinyl ether-tetrafluoroethylene copolymer prepared in this disclosure has excellent mechanical properties, with a tensile strength ≥26MPa and an elongation at break ≥250%; it also has excellent low-temperature resistance, reaching as low as -50℃.

[0032] The solvent water used in this disclosure can be recycled and reused, reducing production costs and making it environmentally friendly. Detailed Implementation

[0033] Embodiments of this disclosure are described in detail below, with examples of these embodiments illustrated in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and intended to explain this disclosure, and should not be construed as limiting it.

[0034] The following embodiments are used to illustrate this disclosure, but are not intended to limit the scope of this disclosure. The detection methods in the following embodiments are as follows:

[0035] (1) Glass transition temperature: DSC, take the median value.

[0036] (2) The vulcanized product TR-10: GB / T7758-2002.

[0037] (3) Low temperature brittleness temperature: GB / T15256-1994.

[0038] (4) Tensile strength: GB / T528-2008.

[0039] (5) Permanent compression set (O-ring, 200℃, 70h): GB / T7759.0-2015.

[0040] (6) Test method for indentation hardness of vulcanized rubber or thermoplastic rubber Part 1: Shore hardness test.

[0041] Example 1

[0042] A method for preparing a fluoroether rubber includes the following steps:

[0043] S1: Add 30kg of high-purity water to a 50L stainless steel polymerization reactor and start stirring at 60rpm. Pour 4kg of pure PMVE and 900g of emulsifier (a mixture of potassium perfluoropolyether carboxylate, polyether oil, and water in a ratio of 10:1:1) into the polymerization reactor. Add A (2000g)CF3CF2CF2CF2O(CF(CF3)CF2O)CF=CF2 and B (1500g)CF3CF2O(CF3CF2O)CF=CF2) to the above microemulsion. Heat to 80℃ until the pressure in the polymerization reactor is about 1.8MPa. Then, add the first mixed gas of PMVE and tetrafluoroethylene to the polymerization reactor until the pressure is 3.0MPa. Add 30g of chain transfer agent 1,2-diiodoethane, 50g of sulfurized monomer 1-iodo-2,2-difluoroethylene, and 6g of initiator potassium persulfate to initiate the copolymerization reaction.

[0044] S2: After the polymerization reaction begins, a second mixed gas of PMVE and TFE is introduced. The molar ratio of PMVE to TFE in the second mixture is 0.5:1. The pressure in the polymerization reactor is maintained at 3.0 MPa. When the consumption of the second mixed monomer reaches 20 kg, the copolymerization reaction is terminated, the polymerization reactor is depressurized, and the elastomer emulsion is obtained. Magnesium chloride aqueous solution is added to the elastomer emulsion for coagulation and washing. The elastomer is then continuously dried in a vacuum drying oven at 120℃ for 4 hours to obtain the low-temperature resistant perfluoroether rubber elastomer product.

[0045] S3: The following compounding components are prepared: (1) 10 kg raw rubber; (2) 0.15 kg triallyl silsesquioxane modified vulcanizing agent; (3) 0.3 kg vulcanizing aid 2,5-di-tert-butylperoxide-2,5-dimethyl ethane; (4) 1.5 kg filler material MT carbon black N9900; (5) 0.5 kg processing aid octadecanoic acid. The above components are added to a mixer and mixed. After standing at room temperature for 20 h, the mixture is re-milled on a two-roll mill to finally obtain perfluoroether rubber vulcanizate.

[0046] The preparation method of triallylsilsesquioxane modified vulcanizing agent is as follows:

[0047] 25 kg of triallyl isocyanurate (TAIC, CAS: 1025-16-2), 0.5 kg of 4,4'-dihydroxy-2,2'-bipyridine / zirconium / lanthanum complex, 0.01 kg of trisilyl alcohol phenyl-cage polysilsesquioxane (CAS: 444315-26-8), 1 kg of stannous octoate, and 200 kg of toluene were added to a sealed stirred reactor. The mixture was stirred at 60 °C for 120 minutes, and the toluene was removed by distillation to obtain triallyl silsesquioxane modified vulcanizing agent.

[0048] The preparation method of the 4,4'-dihydroxy-2,2'-bipyridine / zirconium / lanthanum complex is as follows: 16 kg of 4,4'-dihydroxy-2,2'-bipyridine, 7 kg of zirconium nitrate, 16 kg of lanthanum nitrate, and 200 kg of water are stirred at 40°C for 100 minutes, and the water is removed by distillation to obtain the 4,4'-dihydroxy-2,2'-bipyridine / zirconium / lanthanum complex.

[0049] Table 1 Performance Tests of Perfluoroelastomer Rubber

[0050] Example 2

[0051] A method for preparing a perfluoroether rubber includes the following steps:

[0052] S1: Add 30kg of high-purity water to a 50L stainless steel polymerization reactor and start stirring at 80rpm. Pour 4kg of pure PMVE and 300g of emulsifier (a mixture of perfluoropolyether magnesium carboxylate: polyether oil: water = 1:10:1) into the polymerization reactor. Add A (2000g)CF3CF2CF2CF2O(CF(CF3)CF2O)CF=CF2 and B (1500g)CF3CF2O(CF3CF2O)CF=CF2) to the above microemulsion. Heat to 90℃ until the pressure in the polymerization reactor is about 2.0MPa. Then, add the first mixed gas of PMVE and tetrafluoroethylene to the polymerization reactor until the pressure is 4.0MPa. Add 30g of chain transfer agent 1,2-diiodoethane, 50g of sulfurized monomer 1-iodine-2,2-difluoroethylene, and 6g of initiator potassium persulfate to initiate the copolymerization reaction.

[0053] S2: After the polymerization reaction begins, a second mixed gas of PMVE and TFE is introduced. The molar ratio of PMVE to TFE in the second mixture is 0.5:1. The pressure of the polymerization reactor is maintained at 4.0 MPa. When the consumption of the second mixed monomer reaches 20 kg, the copolymerization reaction is terminated, the polymerization reactor is depressurized and discharged, and the obtained elastomer emulsion is coagulated, washed and dried to obtain perfluoroether rubber.

[0054] S3: The following compounding components are prepared: (1) 10 kg raw rubber; (2) 0.15 kg triallyl silsesquioxane modified vulcanizing agent; (3) 0.3 kg vulcanizing aid 2,5-di-tert-butylperoxide-2,5-dimethyl ethane; (4) 1.5 kg filler material MT carbon black N9900; (5) 0.5 kg processing aid octadecanoic acid. The above components are added to a mixer and mixed. After standing at room temperature for 20 h, the mixture is re-milled on a two-roll mill to finally obtain perfluoroether rubber vulcanizate.

[0055] The preparation method of triallylsilsesquioxane modified vulcanizing agent is as follows:

[0056] 35 kg of triallyl isocyanurate (TAIC, CAS: 1025-16-2), 1 kg of 4,4'-dihydroxy-2,2'-bipyridine / zirconium / lanthanum complex, 0.045 kg of trisilyl alcohol phenyl-cage polysilsesquioxane (CAS: 444315-26-8), 2 kg of stannous octoate, and 250 kg of toluene were added to a sealed stirred reactor. The mixture was stirred at 65°C for 140 minutes, and toluene was removed by distillation to obtain triallyl silsesquioxane modified vulcanizing agent.

[0057] The preparation method of the 4,4'-dihydroxy-2,2'-bipyridine / zirconium / lanthanum complex is as follows: 24 kg of 4,4'-dihydroxy-2,2'-bipyridine, 9 kg of zirconium nitrate, 24 kg of lanthanum nitrate, 250 kg of water, stirred at 45°C for 125 minutes, and the water was removed by distillation to obtain the 4,4'-dihydroxy-2,2'-bipyridine / zirconium / lanthanum complex.

[0058] Table 2 Performance Tests of Perfluoroelastomer Rubber

[0059] Example 3

[0060] A method for preparing a perfluoroether rubber includes the following steps:

[0061] S1: Add 30kg of high-purity water to a 50L stainless steel polymerization reactor and start stirring at 100rpm. Pour 4kg of pure PMVE and 300g of emulsifier (a mixture of sodium perfluoropolyether carboxylate, polyether oil, and water in a ratio of 1:1:10) into the polymerization reactor. Add A (2000g)CF3CF2CF2CF2O(CF(CF3)CF2O)CF=CF2 and B (1500g)CF3CF2O(CF3CF2O)CF=CF2) to the above microemulsion. Heat to 100℃ until the pressure in the polymerization reactor is about 1.5MPa. Then, add the first mixed gas of PMVE and tetrafluoroethylene to the polymerization reactor until the pressure is 3.5MPa. Add 30g of chain transfer agent 1,2-diiodoethane, 50g of sulfurized monomer 1-iodo-2,2-difluoroethylene, and 6g of initiator potassium persulfate to initiate the copolymerization reaction.

[0062] S2: After the polymerization reaction begins, a second mixed gas of PMVE and TFE is introduced. The molar ratio of PPVE to TFE in the second mixture is 0.5:1. The pressure of the polymerization reactor is maintained at 3.5 MPa. When the consumption of the second mixed monomer reaches 20 kg, the copolymerization reaction is terminated, the polymerization reactor is depressurized and discharged, and the obtained elastomer emulsion is coagulated, washed and dried to obtain perfluoroether rubber.

[0063] S3: The following compounding components are prepared: (1) 10 kg raw rubber; (2) 0.15 kg triallyl silsesquioxane modified vulcanizing agent; (3) 0.3 kg vulcanizing aid 2,5-di-tert-butylperoxide-2,5-dimethyl ethane; (4) 1.5 kg filler material MT carbon black N9900; (5) 0.5 kg processing aid octadecanoic acid. The above components are added to a mixer and mixed. After standing at room temperature for 20 h, the mixture is re-milled on a two-roll mill to finally obtain perfluoroether rubber vulcanizate.

[0064] The preparation method of triallylsilsesquioxane modified vulcanizing agent is as follows:

[0065] 40 kg of triallyl isocyanurate (TAIC, CAS: 1025-16-2), 2 kg of 4,4'-dihydroxy-2,2'-bipyridine / zirconium / lanthanum complex, 0.08 kg of trisilyl alcohol phenyl-cage polysilsesquioxane (CAS: 444315-26-8), 2 kg of stannous octoate, and 250 kg of toluene were added to a sealed stirred reactor. The mixture was stirred at 65°C for 160 minutes, and toluene was removed by distillation to obtain triallyl silsesquioxane modified vulcanizing agent.

[0066] The preparation method of the 4,4'-dihydroxy-2,2'-bipyridine / zirconium / lanthanum complex is as follows: 28 kg of 4,4'-dihydroxy-2,2'-bipyridine, 12 kg of zirconium nitrate, 28 kg of lanthanum nitrate, and 250 kg of water are stirred at 45°C for 125 minutes, and the water is removed by distillation to obtain the 4,4'-dihydroxy-2,2'-bipyridine / zirconium / lanthanum complex.

[0067] Table 3 Performance Tests of Perfluoroelastomer Rubber

[0068] Example 4

[0069] A method for preparing a perfluoroether rubber includes the following steps:

[0070] S1: Add 30kg of high-purity water to a 50L stainless steel polymerization reactor and start stirring at 120rpm. Pour 4.5kg of pure PMVE and 300g of emulsifier (a mixture of perfluoropolyether ammonium carboxylate: polyether oil: water = 10:5:5) into the polymerization reactor. Add A (2000g)CF3CF2CF2CF2O(CF(CF3)CF2O)CF=CF2 and B (1500g)CF3CF2O(CF3CF2O)CF=CF2) to the above microemulsion. Heat to 70℃ until the pressure in the polymerization reactor is about 1.5MPa. Then, add the first mixed gas of PMVE and tetrafluoroethylene to the polymerization reactor until the pressure is 3.5MPa. Add 30g of chain transfer agent 1,2-diiodoethane, 50g of sulfurized monomer 1-iodo-2,2-difluoroethylene, and 6g of potassium persulfate to initiate the copolymerization reaction.

[0071] S2: After the polymerization reaction begins, a second mixed gas of PMVE and TFE is introduced. The molar ratio of PMVE to TFE in the second mixture is 0.5:1. The pressure of the polymerization reactor is maintained at 3.5 MPa. When the consumption of the second mixed monomer reaches 20 kg, the copolymerization reaction is terminated, the polymerization reactor is depressurized and discharged, and the obtained elastomer emulsion is coagulated, washed and dried to obtain perfluoroether rubber.

[0072] S3: The following compounding components are prepared: (1) 10 kg raw rubber; (2) 0.15 kg triallyl silsesquioxane modified vulcanizing agent; (3) 0.3 kg vulcanizing aid 2,5-di-tert-butylperoxide-2,5-dimethyl ethane; (4) 1.5 kg filler material MT carbon black N9900; (5) 0.5 kg processing aid octadecanoic acid. The above components are added to a mixer and mixed. After standing at room temperature for 20 h, the mixture is re-milled on a two-roll mill to finally obtain perfluoroether rubber vulcanizate.

[0073] The preparation method of triallylsilsesquioxane modified vulcanizing agent is as follows:

[0074] 50 kg of triallyl isocyanurate (TAIC, CAS: 1025-16-2), 2.5 kg of 4,4'-dihydroxy-2,2'-bipyridine / zirconium / lanthanum complex, 0.1 kg of trisilyl alcohol phenyl-cage polysilsesquioxane (CAS: 444315-26-8), 3 kg of stannous octoate, and 300 kg of toluene were added to a sealed stirred reactor. The mixture was stirred at 70 °C for 180 minutes, and the toluene was removed by distillation to obtain triallyl silsesquioxane modified vulcanizing agent.

[0075] The preparation method of the 4,4'-dihydroxy-2,2'-bipyridine / zirconium / lanthanum complex is as follows: 32 kg of 4,4'-dihydroxy-2,2'-bipyridine, 14 kg of zirconium nitrate, 32 kg of lanthanum nitrate, and 300 kg of water are stirred at 50°C for 150 minutes, and the water is removed by distillation to obtain the 4,4'-dihydroxy-2,2'-bipyridine / zirconium / lanthanum complex.

[0076] Table 4 Performance Tests of Perfluoroelastomer Rubber

[0077] Comparative Example 1

[0078] A method for preparing a fluoroether rubber includes the following steps:

[0079] S1: Add 30kg of high-purity water to a 50L stainless steel polymerization reactor and start stirring at 60rpm. Pour 4kg of pure PMVE and 900g of emulsifier (a mixture of potassium perfluoropolyether carboxylate, polyether oil, and water in a ratio of 10:1:1) into the polymerization reactor. Add A (2000g)CF3CF2CF2CF2O(CF(CF3)CF2O)CF=CF2 and B (1500g)CF3CF2O(CF3CF2O)CF=CF2) to the above microemulsion. Heat to 80℃ until the pressure in the polymerization reactor is about 1.8MPa. Then, add the first mixed gas of PMVE and tetrafluoroethylene to the polymerization reactor until the pressure is 3.0MPa. Add 30g of chain transfer agent 1,2-diiodoethane, 50g of sulfurized monomer 1-iodo-2,2-difluoroethylene, and 6g of initiator potassium persulfate to initiate the copolymerization reaction.

[0080] S2: After the polymerization reaction begins, a second mixed gas of PMVE and TFE is introduced. The molar ratio of PMVE to TFE in the second mixture is 0.5:1. The pressure in the polymerization reactor is maintained at 3.0 MPa. When the consumption of the second mixed monomer reaches 20 kg, the copolymerization reaction is terminated, the polymerization reactor is depressurized, and the elastomer emulsion is obtained. Magnesium chloride aqueous solution is added to the elastomer emulsion for coagulation and washing. The elastomer is then continuously dried in a vacuum drying oven at 120℃ for 4 hours to obtain the low-temperature resistant perfluoroether rubber elastomer product.

[0081] S3: The following compounding components are prepared: (1) 10 kg raw rubber; (2) 0.15 kg vulcanizing agent triallyl isocyanurate; (3) 0.3 kg vulcanizing aid 2,5-di-tert-butylperoxide-2,5-dimethylethane; (4) 1.5 kg filler MT carbon black N9900; (5) 0.5 kg processing aid octadecanoic acid. The above components are added to a mixer and mixed. After standing at room temperature for 20 h, the mixture is re-milled on a two-roll mill to finally obtain perfluoroether rubber vulcanizate.

[0082] Table 5 Performance Tests of Perfluoroelastomer Rubber

[0083] Comparative Example 2

[0084] A method for preparing a fluoroether rubber includes the following steps:

[0085] S1: Add 30kg of high-purity water to a 50L stainless steel polymerization reactor and start stirring at 60rpm. Pour 4kg of pure PMVE and 900g of emulsifier (a mixture of potassium perfluoropolyether carboxylate, polyether oil, and water in a ratio of 10:1:1) into the polymerization reactor. Add A (2000g)CF3CF2CF2CF2O(CF(CF3)CF2O)CF=CF2 and B (1500g)CF3CF2O(CF3CF2O)CF=CF2) to the above microemulsion. Heat to 80℃ until the pressure in the polymerization reactor is about 1.8MPa. Then, add the first mixed gas of PMVE and tetrafluoroethylene to the polymerization reactor until the pressure is 3.0MPa. Add 30g of chain transfer agent 1,2-diiodoethane, 50g of sulfurized monomer 1-iodo-2,2-difluoroethylene, and 6g of initiator potassium persulfate to initiate the copolymerization reaction.

[0086] S2: After the polymerization reaction begins, a second mixed gas of PMVE and TFE is introduced. The molar ratio of PMVE to TFE in the second mixture is 0.5:1. The pressure in the polymerization reactor is maintained at 3.0 MPa. When the consumption of the second mixed monomer reaches 20 kg, the copolymerization reaction is terminated, the polymerization reactor is depressurized, and the elastomer emulsion is obtained. Magnesium chloride aqueous solution is added to the elastomer emulsion for coagulation and washing. The elastomer is then continuously dried in a vacuum drying oven at 120℃ for 4 hours to obtain the low-temperature resistant perfluoroether rubber elastomer product.

[0087] S3: The following compounding components are prepared: (1) 10 kg raw rubber; (2) 0.15 kg triallyl silsesquioxane modified vulcanizing agent; (3) 0.3 kg vulcanizing aid 2,5-di-tert-butylperoxide-2,5-dimethyl ethane; (4) 1.5 kg filler material MT carbon black N9900; (5) 0.5 kg processing aid octadecanoic acid. The above components are added to a mixer and mixed. After standing at room temperature for 20 h, the mixture is re-milled on a two-roll mill to finally obtain perfluoroether rubber vulcanizate.

[0088] The preparation method of triallylsilsesquioxane modified vulcanizing agent is as follows:

[0089] 25 kg of triallyl isocyanurate (TAIC, CAS: 1025-16-2), 0.01 kg of trisilyl phenyl-cage polysilsesquioxane (CAS: 444315-26-8), 1 kg of stannous octoate, and 200 kg of toluene were added to a sealed stirred reactor. The mixture was stirred at 60 °C for 120 minutes, and the toluene was removed by distillation to obtain the triallyl silsesquioxane modified vulcanizing agent.

[0090] Table 6 Performance Tests of Perfluoroelastomer Rubber

[0091] As can be seen from the above specific embodiments, the low-temperature resistant perfluoroether rubber prepared by this method has excellent mechanical properties, low-temperature resistance and sulfurization properties.

[0092] The applicant declares that the above embodiments are used to further illustrate this disclosure, but this disclosure is not limited to the above embodiments, that is, it does not mean that this disclosure must rely on the above embodiments to be implemented. Those skilled in the art should understand that any improvements to this disclosure, equivalent substitutions of the raw materials of the disclosed products, additions of auxiliary components, and selection of specific methods, etc., all fall within the protection scope and disclosure scope of this disclosure.

Claims

1. A method for preparing and applying low-temperature resistant high-purity perfluoroether rubber, the operation steps of which are as follows: S1: According to the weight percentage, add 300-400 parts of high-purity water to the polymerization reactor, start stirring and add 0.5-2 parts of microemulsion, add 0.25-0.45 parts of comonomers A and B to the microemulsion, stir at 30-120 rpm, heat the polymerization reactor while introducing PMVE, until the temperature reaches 80-120℃ and the pressure reaches 1.5-1.8 MPa, then introduce the first mixed gas of PMVE and TFE until the pressure in the polymerization reactor reaches 3.0-5.0 MPa, add 0.05-0.2 parts of chain transfer agent, 0.02-0.1 parts of sulfurization point monomer, and 0.01-0.1 parts of initiator to initiate the copolymerization reaction; S2: After the polymerization reaction begins, a second mixed gas of PMVE and TFE is introduced to maintain the pressure of the polymerization reactor at 3.0-5.0 MPa and the temperature at 80-120℃. When the consumption of the second mixed monomer reaches 30-50 parts, the copolymerization reaction is terminated, the polymerization reactor is depressurized and discharged, and the obtained elastomer emulsion is coagulated, washed and dried to obtain perfluoroether rubber. S3: The following compounding components are prepared: (1) 10-12 parts raw rubber; (2) 0.15-0.18 parts triallyl silsesquioxane modified vulcanizing agent; (3) 0.3-0.5 parts vulcanizing aid 2,5-di-tert-butylperoxide-2,5-dimethylethane; (4) 1.5-2 parts filler material MT carbon black N9900; (5) 0.5-0.8 parts processing aid octadecanoic acid. The above components are added to a mixer and mixed. After being placed at room temperature for 20 hours, the mixture is re-milled on a two-roll mill to finally obtain perfluoroether rubber vulcanizate.

2. The method for preparing and applying a low-temperature resistant high-purity perfluoroether rubber according to claim 1, wherein the mass ratio of the microemulsion is emulsifier:polyether oil:water = 10:1 to 1:10 to 1:

10.

3. The method for preparing and applying a low-temperature resistant high-purity perfluoroether rubber according to claim 2, wherein the emulsifier is selected from potassium perfluoroether carboxylate, magnesium perfluoroether carboxylate, sodium perfluoroether carboxylate, and ammonium perfluoroether carboxylate; and the polyether oil is selected from PFPE, with the structural formula (—CF2—O—CF2—)n.

4. A method for preparing and applying a low-temperature resistant high-purity perfluoroether rubber according to any one of claims 1-3, wherein the comonomer A is selected from CF3CF2CF2CF2O (CF(CF3)CF2O). n CF = CF2, n = 0-6, n = 1-3 is optional; the comonomer B is selected from CF3CF2O (CF3CF2O). m CF = CF2, m = 0-5, m = 1-3 can be selected.

5. A method for preparing and applying a low-temperature resistant high-purity perfluoroether rubber according to any one of claims 1-4, wherein the chain transfer agent is selected from iodoalkanes, alkane compounds, alcohols, esters, and organohalides, including one or a combination of 1,3-diiodoperfluoropropane, 1,4-diiodoperfluorobutane, 1,3-diiodo-2-chloroperfluoropropane, 1,5-diiodo-2,4-dichloroperfluoropentane, 1,3-diiodoperfluorobutane, 1,6-diiodoperfluorohexane, 1,8-diiodoperfluorooctane, perfluoroisopropyl iodine, perfluoron-butyl iodine, trifluoromethyl iodine, methyl iodine, isopentane, methanol, isopropanol, ethyl acetate, diethyl malonate, CCl4, CBrCl3, CF2BrCFBrCF3, and CF2I2.

6. A method for preparing and applying a low-temperature resistant high-purity perfluoroether rubber according to any one of claims 1-5, wherein the vulcanizing point monomer is selected from chlorinated olefins, including one or a combination of several of the following: trifluoroethylene bromide, 4-bromoperfluoro-1-butene, 1-bromo-2,2-difluoroethylene, 4-bromo-3,3,4,4-tetrafluoro-1-butene, perfluoroalkyl bromide, 4-bromo-1,1,2-trifluoro-1-butene, and 4-bromo-1,1,3,3,4,4-hexafluoro-1-butene.

7. A method for preparing and applying a low-temperature resistant high-purity perfluoroether rubber according to any one of claims 1-5, wherein the initiator is selected from one or a combination of several of diisopropyl peroxide, benzoyl peroxide, isopropylbenzene peroxide, tert-butyl hydroperoxide, potassium persulfate, and ammonium persulfate.

8. A method for preparing and applying a low-temperature resistant high-purity perfluoroether rubber according to any one of claims 1-7, wherein the molar ratio of PMVE to TFE in the first mixed gas is 1:1.0-2.0; the molar ratio of PMVE to TFE in the second mixed gas is 1:1.5-2.0; and the purity of the PMVE and TFE monomers is not less than 99.99%.

9. The method for preparing and use of low temperature resistant high purity perfluoroether rubber according to any one of claims 1-8, characterized in that: The preparation method of the triallylsilsesquioxane modified vulcanizing agent is as follows: By weight, add 25-50 parts of triallyl isocyanurate (TAIC), 0.5-2.5 parts of 4,4'-dihydroxy-2,2'-bipyridine / zirconium / lanthanum complex, 0.01-0.1 parts of trisilyl phenyl-cage polysilsesquioxane, 1-3 parts of stannous octoate, and 200-300 parts of toluene to a sealed stirred reactor. Stir at 60-70°C for 120-180 minutes, and remove the toluene by distillation to obtain the triallyl silsesquioxane modified vulcanizing agent.

10. The method for preparing and use of low temperature resistant high purity perfluoroether rubber according to claim 9, characterized in that: The preparation method of the 4,4'-dihydroxy-2,2'-bipyridine / zirconium / lanthanum complex is as follows: 16-32 parts of 4,4'-dihydroxy-2,2'-bipyridine, 7-14 parts of zirconium nitrate, 16-32 parts of lanthanum nitrate, 200-300 parts of water, stirred at 40-50℃ for 100-150 minutes, and the water was removed by distillation to obtain the 4,4'-dihydroxy-2,2'-bipyridine / zirconium / lanthanum complex.