Wafer and metal bump bonded structure and manufacturing process therefor
By forming a bonding structure of supporting frame and metal bumps on a metal sheet, the problem of insufficient metal layer thickness in traditional processes is solved, realizing high-strength, low-cost wafer-to-metal bump bonding, improving the chip's current carrying capacity and heat dissipation, and making it suitable for applications with small bonding areas and height differences.
Patent Information
- Application Number
- PCT/CN2025/128715
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-16
- Filing Date
- 2025-10-20
- Publication Date
- 2026-11-19
AI Technical Summary
In the manufacturing process of traditional semiconductor devices, the metal layer thickness in the chip lead bonding area is insufficient, which leads to problems such as metal layer damage and cracking. In addition, the existing process is not suitable for small bonding areas and copper sheets with height differences, resulting in inconvenience in applying adhesive and operation.
A wafer-to-metal bump bonding structure fabrication process is adopted, which involves forming a support frame and metal bumps on a metal sheet, combining wet or dry slurry processes to achieve bonding between the metal bumps and the wafer, and forming a reliable bonding structure through pressure sintering and molding.
It improves the chip's current carrying capacity and heat dissipation capacity, enhances the bonding strength and reliability of the metal layer, simplifies the operation process, and reduces costs, making it particularly suitable for third-generation silicon carbide power semiconductor devices.
Smart Images

Figure CN2025128715_19112026_PF_FP_ABST
Abstract
Description
A wafer-to-metal bump bonding structure and its fabrication process Technical Field
[0001] This invention belongs to the field of chip manufacturing technology, and specifically discloses a wafer-metal bump bonding structure and its manufacturing process. Background Technology
[0002] Patent application number CN106170856A, entitled "A support and clip having a sinterable curable paste for connecting to semiconductor elements, sinterable paste, manufacturing process and use," discloses a process of pre-coating a sinterable paste onto a bonding copper sheet, then placing it on the chip bonding area, and forming a bond between the chip and the pin through a pressure sintering process. This process has relatively strict requirements on the size of the chip bonding area. Due to the limitations of the adhesive coating process, it is not suitable for smaller bonding areas (usually less than 2mm × 2mm), and there are problems such as copper sheet drift causing short circuits and inconvenience in operation. In addition, there are problems with adhesive coating for copper sheets with height differences.
[0003] Patent application number TW202345248A, entitled "Sintering-Ready Multilayer Line / Tape Pads and Process for Top-Attachment of Diodes," discloses a process of pre-coating on a copper sheet and then sintering to the chip bonding area using pressure sintering. Due to the limitations of the pre-coating process, there are also size requirements for the chip bonding area, and it is not suitable for smaller bonding areas. In addition, due to the characteristics of the pre-coated metal film, a protective film needs to be covered on the exposed side of the metal film after pre-coating to prevent damage or oxidation failure of the metal film during the transfer process. This causes problems of metal film damage and inconvenience in the subsequent film peeling process. Summary of the Invention
[0004] The purpose of this invention is to overcome the shortcomings of existing technologies and provide a wafer-to-metal bump bonding structure and its fabrication process. This solves the problems of metal layer damage and cracking caused by insufficient metal layer thickness in the chip lead bonding area during the fabrication of traditional semiconductor devices. At the same time, it provides sufficient metal bump thickness to facilitate the bonding of thick copper wires or thick copper sheets, or flip-chip bonding onto the substrate, thereby improving the chip's current carrying capacity and heat dissipation capacity. Compared with traditional processes, this invention has a simple process, high metal layer bonding strength, high reliability, and low cost, and has broad application prospects, especially in the field of power semiconductor devices based on third-generation semiconductor silicon carbide.
[0005] The technical solution adopted in this invention is:
[0006] A fabrication process for a wafer-to-metal bump bonding structure, wherein the process includes the following steps:
[0007] Step S1: Provide metal sheets and wafers;
[0008] Step S2: Attach a support film to one side of the metal sheet, chemically etch a sintering surface on the other side of the metal sheet, form a support frame around the sintering surface, and form multiple spaced metal bumps inside the support frame of the sintering surface. Clean the surface to obtain metal bumps with a support frame and a support film.
[0009] Step S3: Form a paste layer on the wire bonding area of the wafer and place one side of the metal bump on the paste layer; or form a dry paste film on the sintering surface of the metal bump and place one side of the dry paste film on the wire bonding area of the wafer.
[0010] Step S4: Sinter the metal bumps from step S3 with the wafer, and remove the support film and support frame to obtain a bonding structure;
[0011] Step S5: Cut and separate the bonding structure into individual chips.
[0012] Preferably, in the fabrication process of the wafer and metal bump bonding structure, the material of the metal sheet in step S1 is selected from copper, copper-molybdenum alloy, and tungsten-copper alloy, and the thickness of the metal sheet is 50-300 micrometers; step S2 further includes: electroplating silver on the sintering surface of the metal sheet to form a sintering surface with a silver layer, and the thickness of the silver layer is 1-4 micrometers.
[0013] Preferably, the fabrication process of the wafer-metal bump bonding structure, wherein step S3, which involves fabricating a paste layer on the wire bonding area of the wafer and placing one side of the metal bump on the paste layer, specifically includes the following steps:
[0014] Step S31: Mix the metal particles, solvent and sintering accelerator to obtain a wet slurry;
[0015] Step S32: Apply a layer of wet paste to the wire bonding area of the wafer by screen printing or dispensing to form a paste layer with a thickness of 10-200 micrometers;
[0016] Step S33: Place one side of the metal bump on the slurry layer.
[0017] Preferably, in the fabrication process of the wafer-metal bump bonding structure, step S4 specifically includes the following steps:
[0018] The metal bumps and the wafer from step S3 are transferred to an oxygen-free oven, filled with nitrogen, and the oxygen content is controlled to be below 50 ppm. The temperature is raised to 150°C within 0.5 h and held for 0.5 h. Then, the temperature is raised to 220°C within 0.5 h and held for 1 h. After that, the support film and support frame are removed at 220°C to obtain the bonding structure.
[0019] Preferably, the fabrication process of the wafer-metal bump bonding structure, wherein step S3, which involves fabricating a paste layer on the wire bonding area of the wafer and placing one side of the metal bump on the paste layer, specifically includes the following steps:
[0020] Step S31: Mix the metal particles, solvent and sintering accelerator to obtain a wet slurry;
[0021] Step S32: Apply a layer of wet paste to the wire bonding area of the wafer by screen printing or dispensing to form a paste layer with a thickness of 10-200 micrometers;
[0022] Step S33: Transfer the wafer coated with the slurry layer to an oxygen-free oven, fill it with nitrogen, control the oxygen content to be below 50 ppm, raise the temperature to 150°C within 0.5 h and keep it for 1 h to obtain a semi-cured slurry layer.
[0023] Step S34: Place one side of the metal bump on the semi-cured slurry layer.
[0024] Preferably, the fabrication process of the wafer-metal bump bonding structure, wherein step S3, which involves forming a dry paste film on the sintering surface of the metal bump and placing one side of the dry paste film on the wire bonding area of the wafer, specifically includes the following steps:
[0025] Step S31: Mix the metal particles, solvent and sintering accelerator to obtain a wet slurry;
[0026] Step S32: Transfer the wet paste onto the support film using a screen printing process;
[0027] Step S33: Transfer the wet slurry and the supporting film to an oven, raise the temperature to 100-150℃ in 0.5 hours, maintain the temperature for 1-3 hours, and obtain the dry slurry film;
[0028] Step S34: The dry slurry film is bonded to the side of the metal bump with the sintered surface by pressure transfer.
[0029] Step S35: Place one side of the dry slurry film on the wire bonding area of the wafer.
[0030] Preferably, in the fabrication process of the wafer-metal bump bonding structure, the metal particles in step S31 are selected from silver particles or copper particles, the particle size of the metal particles is 50nm-100nm, the solvent is an alcohol or ether organic compound with a carbon chain of 4-8, and the sintering promoter is an aliphatic amine with a decomposition temperature of about 150°C.
[0031] Preferably, in the fabrication process of the wafer-metal bump bonding structure, step S4 specifically includes:
[0032] The metal bumps from step S3 are transferred together with the wafer transfer and pressure sintering fixture into a pressure sintering machine for sintering. Then, the support film and support frame are removed to obtain the bonding structure. The sintering temperature is 230-280℃, the sintering time is 150-250 seconds, the sintering pressure is 8-20 MPa, and the temperature at which the support film is removed is 220℃.
[0033] Preferably, the manufacturing process of the wafer-metal bump bonding structure further includes a molding step after step S4, which specifically involves filling the gap between the wafer and the metal bump in the bonding structure with epoxy resin and molding it with a transfer film to obtain a transfer-molded bonding structure. The molding temperature is 110-150℃ and the molding time is 50-150s.
[0034] A wafer-to-metal bump bonding structure is fabricated using a wafer-to-metal bump bonding structure fabrication process.
[0035] The present invention has the following advantages:
[0036] (1) The wafer and metal bump bonding structure fabrication process of the present invention solves the problems of metal layer damage and cracking caused by insufficient metal layer thickness in the chip lead bonding area during the fabrication of traditional semiconductor devices. By controlling the thickness of the metal bump to 50-300 micrometers, the metal bump is easy to bond with thick copper wire, thereby improving the current carrying capacity and heat dissipation capacity of the chip.
[0037] (2) The wafer and metal bump bonding structure of the present invention is fabricated by bonding the metal layer to the chip lead area through a reliable sintering process, and filling the gap between the metal layer and the wafer with epoxy resin sealant to protect the isolation area, interconnect layer and passivation layer of the chip and improve the reliability of the chip in subsequent use.
[0038] (3) The wafer-metal bump bonding structure fabrication process of the present invention achieves wafer-level coverage of metal support film with a thickness of more than 100 micrometers, providing reliable support for subsequent coarse copper wire bonding; significantly improves the current carrying capacity and heat dissipation capacity of the chip, especially the silicon carbide chip; reliable sintering layer and epoxy resin sealant protect the isolation area, interconnect area and passivation area of the wafer, improving the reliability of the wafer.
[0039] (4) The wafer and metal bump bonding structure of the present invention is easy to operate and economical; the electrode of the chip is led out by the copper sheet, and the gap between the wafer and the copper sheet is protected by epoxy resin sealant. It can be directly applied to the PCB board, eliminating the need for packaging support and improving the convenience and economy of chip use. Attached Figure Description
[0040] Figure 1 is a schematic diagram of the structure of Example 1 in which a support film is attached to one side of a metal sheet.
[0041] Figure 2 is a schematic diagram of the structure of forming a supporting frame on one side of the metal sheet in Embodiment 1.
[0042] Figure 3 is a schematic diagram of the structure of the wire bonding region of the wafer covered with a paste layer in Example 1.
[0043] Figure 4 is a schematic diagram of the structure of the metal bumps placed on the slurry layer in Example 1.
[0044] Figure 5 is a schematic diagram of the wafer-metal bump bonding structure of Example 1.
[0045] Figure 6 is a schematic diagram of the bonding structure of the transfer encapsulation in Example 1.
[0046] Figure 7 is a schematic diagram of the structure of a single chip separated from the bonding structure in Example 1.
[0047] Figure 8 is a schematic diagram of the structure of Example 2 in which a support film is attached to one side of a metal sheet.
[0048] Figure 9 is a schematic diagram of the structure of the wire bonding region of the wafer covered with a paste layer in Example 2.
[0049] Figure 10 is a schematic diagram of the structure of metal bumps placed on a semi-cured slurry layer in Example 2.
[0050] Figure 11 is a schematic diagram of the wafer-metal bump bonding structure in Example 2.
[0051] Figure 12 is a schematic diagram of the bonding structure of the transfer encapsulation in Example 2.
[0052] Figure 13 is a schematic diagram of the structure of a single chip separated from the bonding structure in Example 2.
[0053] Figure 14 is a schematic diagram of the structure of Example 3 in which a support film is attached to one side of a metal sheet.
[0054] Figure 15 is a schematic diagram of the structure of Example 3 in which wet slurry is applied to the support membrane.
[0055] Figure 16 is a schematic diagram of the structure of the dry slurry film of Example 3 bonded to the metal bump.
[0056] Figure 17 is a schematic diagram of the structure of the metal bumps placed in the wire bonding area of the wafer in Example 3.
[0057] Figure 18 is a schematic diagram of the wafer-metal bump bonding structure in Example 3.
[0058] Figure 19 is a schematic diagram of the bonding structure of the transfer encapsulation in Example 3.
[0059] Figure 20 is a schematic diagram of the structure of a single chip separated from the bonding structure in Example 3.
[0060] Figure 21 is a perspective view of a metal protrusion with a supporting frame and a supporting membrane.
[0061] Figure 22 is a three-dimensional schematic diagram of the wafer-metal bump bonding structure. Detailed Implementation
[0062] The present invention will be further described in detail below with reference to the accompanying drawings and embodiments. Unless otherwise stated, the terminology used herein should be understood in accordance with the conventional usage of those skilled in the art.
[0063] As used herein, a support film is attached to one side of the metal sheet. The support film is made of polyimide, and the preferred metal sheet material is copper, with grades such as C7025 or EFTET64. In some applications requiring a low coefficient of thermal expansion, copper-molybdenum alloy or tungsten-copper alloy can be selected. The thickness of the metal sheet is preferably 50-300 micrometers, more preferably 100 micrometers. Thicknesses exceeding 300 micrometers can also be used, but with greater residual stress. The sintered surface of the metal sheet can be silver-plated, with a silver layer thickness of 1-4 micrometers, preferably 3 micrometers.
[0064] Preferably, the wet slurry of the present invention comprises 60-80% metal particles, 20-30% solvent, and 1-5% sintering accelerator. The metal particles are silver or copper particles with an average particle size of 50 nm and a maximum particle size of no more than 100 nm. The solvent is an alcohol or ether organic compound with a carbon chain of 4-8. The sintering accelerator is an aliphatic amine with a decomposition temperature of about 150 degrees Celsius. Specifically, the solvent includes 60-70% isobutanol, 20-30% 2-pentanone, and 5-10% propylene glycol methyl ether or isopropanol. The sintering accelerator can be an amine inorganic compound such as hexadecylamine, octadecylamine, or dodecylamine.
[0065] One side of the metal sheet is chemically etched to form a sintered surface. A supporting frame is formed around the sintered surface. Multiple spaced metal protrusions are formed inside the supporting frame of the sintered surface. The supporting frame can be circular, square, or other shapes that can provide support.
[0066] Example 1
[0067] A fabrication process for a wafer-to-metal bump bonding structure, the process comprising the following steps:
[0068] Step S1: Provide a metal sheet 9 and a wafer 4. The metal sheet is made of copper, grade C7025, and the thickness of the metal sheet is 100 micrometers.
[0069] Step S2: As shown in Figure 1, a support film 2 is attached to one side of the metal sheet 9. As shown in Figure 2, a sintering surface is formed by chemical etching on the other side of the metal sheet 9. A support frame 1 is formed on the outer periphery of the sintering surface. Multiple spaced metal bumps 3 are formed inside the support frame 1 of the sintering surface. Silver is electroplated on the sintering surface of the metal sheet 9 to form a sintering surface with a silver layer. The thickness of the silver layer is 3 micrometers. After cleaning, metal bumps 3 with support frame 1 and support film 2 are obtained. A three-dimensional view of metal bumps 3 with support frame 1 and support film 2 is shown in Figure 21. Multiple spaced metal bumps 3 are formed inside the support frame 1.
[0070] Step S3: A paste layer 5 is formed on the wire bonding area of the wafer 4, and one side of the metal bump 3 is placed on the paste layer 5.
[0071] Step S3 specifically includes the following steps:
[0072] Step S31: Mix 70% metal particles, 25% solvent and 5% sintering accelerator by mass percentage to obtain a wet slurry. The metal particles are copper particles with a particle size of 50 nm. The solvent includes 65% isobutanol, 25% 2-pentanone and 10% propylene glycol methyl ether. The sintering accelerator is hexadecylamine.
[0073] Step S32, as shown in Figure 3, a layer of wet paste is applied to the wire bonding area of wafer 4 by screen printing or dispensing to form paste layer 5, the thickness of paste layer 5 being 100 micrometers.
[0074] Step S33, as shown in Figure 4, place one side of the metal bump 3 on the slurry layer 5;
[0075] Step S4: Transfer the metal bump 3 and the wafer 4 from step S3 to an oxygen-free oven, fill with nitrogen, control the oxygen content to below 50 ppm, raise the temperature to 150°C within 0.5 h and hold for 0.5 h, then raise the temperature to 220°C within 0.5 h and hold for 1 h, and then at 220°C, as shown in Figure 5, remove the support film 2 and the support frame 1 to obtain the wafer-metal bump bonding structure. A three-dimensional schematic diagram of the bonding structure is shown in Figure 22.
[0076] Step S5, as shown in Figure 6, fill the gap between wafer 4 and copper sheet in the bonding structure with epoxy resin powder, and then encapsulate it with a transfer film. The encapsulation temperature is 150℃ and the encapsulation time is 100s. Use mechanical grinding to remove excess encapsulation material and expose the copper sheet.
[0077] Step S6, as shown in Figure 7, involves separating the transfer-molded bonding structure into individual chips using a wafer separator. The separated chips include a metal sheet 9, a wafer 4, sintering paste, and epoxy resin sealant 8. The metal sheet 9 is bonded to the lead bonding area of the wafer 4 using the sintering paste, and the epoxy resin sealant fills the gap between the wafer and the metal sheet to provide a sealing effect.
[0078] Example 2
[0079] A fabrication process for a wafer-to-metal bump bonding structure, the process comprising the following steps:
[0080] Step S1: Provide a metal sheet 9 and a wafer 4. The metal sheet is made of copper, grade C7025, and the thickness of the metal sheet 9 is 100 micrometers.
[0081] Step S2, as shown in Figure 8, a support film 2 is attached to one side of the metal sheet 9, and a sintering surface is formed by chemical etching on the other side of the metal sheet 9. A support frame 1 is formed on the outer periphery of the sintering surface, and multiple spaced metal bumps 3 are formed inside the support frame 1 of the sintering surface. Silver is electroplated on the sintering surface of the metal sheet 9 to form a sintering surface with a silver layer. The thickness of the silver layer is 3 micrometers. After cleaning, metal bumps 3 with support frame 1 and support film are obtained.
[0082] Step S3: A paste layer 5 is formed on the wire bonding area of the wafer, and one side of the metal bump 3 is placed on the paste layer 5.
[0083] Step S3 specifically includes the following steps:
[0084] Step S31: Mix 70% metal particles, 25% solvent and 5% sintering accelerator by mass percentage to obtain a wet slurry. The metal particles are copper particles with a particle size of 50 nm. The solvent includes 65% isobutanol, 25% 2-pentanone and 10% propylene glycol methyl ether. The sintering accelerator is hexadecylamine.
[0085] Step S32, as shown in Figure 9, a layer of wet paste is applied to the wire bonding area of wafer 4 by screen printing or dispensing to form a paste layer 5 with a thickness of 100 micrometers.
[0086] Step S33: Transfer the wafer 4 coated with slurry layer 5 to an oxygen-free oven, fill it with nitrogen, control the oxygen content to be below 50 ppm, raise the temperature to 150°C within 0.5 h and keep it for 1 h to obtain a semi-cured slurry layer 5.
[0087] Step S34, as shown in Figure 10, place one side of the metal bump 3 on the semi-cured slurry layer 5.
[0088] Step S4: The metal bump 3 and the wafer 4 from step S3 are transferred together to the pressure sintering fixture and sintered in a pressure sintering machine, as shown in Figure 11. Then, the support film 2 and the support frame 1 are removed to obtain the bonding structure. The sintering temperature is 250°C, the sintering time is 180 seconds, the sintering pressure is 12 MPa, and the temperature at which the support film 2 and the support frame 1 are removed is 220°C.
[0089] Step S5, as shown in Figure 12, fill the gap between wafer 4 and copper sheet in the bonding structure with epoxy resin powder, and then encapsulate it with a transfer film. The encapsulation temperature is 150℃ and the encapsulation time is 100s. Use mechanical grinding to remove excess encapsulation material and expose the copper sheet.
[0090] Step S6: As shown in Figure 13, the bonding structure of the transfer encapsulation is cut and separated into individual chips by a wafer separator. The separated chip includes a metal sheet 9, a wafer 4, a sintering paste and an epoxy resin sealant 8. The metal sheet is bonded to the wafer lead bonding area by the sintering paste, and the epoxy resin sealant fills the gap between the wafer and the metal sheet to play a sealing role.
[0091] Example 3
[0092] A fabrication process for a wafer-to-metal bump bonding structure, the process comprising the following steps:
[0093] Step S1: Provide a metal sheet 9 and a wafer 4. The metal sheet is made of copper, grade C7025, and the thickness of the metal sheet is 100 micrometers.
[0094] Step S2, as shown in Figure 14, a support film 2 is attached to one side of the metal sheet 9, and a sintering surface is formed by chemical etching on the other side of the metal sheet 9. A support frame 1 is formed on the outer periphery of the sintering surface, and a plurality of spaced metal bumps 3 are formed inside the support frame 1 of the sintering surface. Silver is electroplated on the sintering surface of the metal sheet 9 to form a sintering surface with a silver layer. The thickness of the silver layer is 3 micrometers. After cleaning, metal bumps 3 with support frame 1 and support film are obtained.
[0095] Step S3: A dry paste film 6 is formed on the sintering surface of the metal bump 3, and one side of the dry paste film 6 is placed on the wire bonding area of the wafer 4.
[0096] Step S3 specifically includes the following steps:
[0097] Step S31: Mix 70% metal particles, 25% solvent and 5% sintering accelerator by mass percentage to obtain a wet slurry. The metal particles are copper particles with a particle size of 50 nm. The solvent includes 65% isobutanol, 25% 2-pentanone and 10% propylene glycol methyl ether. The sintering accelerator is hexadecylamine.
[0098] Step S32, as shown in Figure 15, the wet paste is transferred onto the support film 7 by screen printing.
[0099] Step S33: Transfer the wet slurry and the supporting film 7 into an oven, raise the temperature to 120°C in 0.5 hours, maintain the temperature for 1 hour, and obtain the dry slurry film 6.
[0100] Step S34, as shown in Figure 16, the dry slurry film 6 is bonded to the side of the metal bump 3 with the sintered surface by pressure transfer.
[0101] Step S35, as shown in Figure 17, place one side of the dry slurry film 6 on the wire bonding area of the wafer 3;
[0102] Step S4: The metal bump 3 and the wafer 4 from step S3 are transferred together to the pressure sintering fixture and sintered in a pressure sintering machine. The pressure sintering fixture is a tray, as shown in Figure 18. Then, the support film 2 and the support frame 1 are removed to obtain the bonding structure. The sintering temperature is 250°C, the sintering time is 180 seconds, the sintering pressure is 12 MPa, and the temperature at which the support film and the support frame are removed is 220°C.
[0103] Step S5, as shown in Figure 19, fill the gap between wafer 4 and copper sheet in the bonding structure with epoxy resin powder, and then encapsulate it with a transfer film. The encapsulation temperature is 150℃ and the encapsulation time is 100s. Use mechanical grinding to remove excess encapsulation material and expose the copper sheet.
[0104] Step S6, as shown in Figure 20, the bonding structure of the transfer encapsulation is cut and separated into individual chips by a wafer separator. The separated chip includes metal bumps 3, wafer 4, sintering paste and epoxy resin sealant 8. The metal sheet is bonded to the wafer lead bonding area by the sintering paste, and the epoxy resin sealant fills the gap between the wafer and the metal sheet to play a sealing role.
[0105] Traditional method: The chip surface metal is aluminum-silicon-copper with a thickness of 5 micrometers, the bonding copper sheet is 10 millimeters thick, and the package type is TO247.
[0106] Comparative Example 1
[0107] The patent application number is CN106170856A, and the patent title is a patent application for a support and clip having a sinterable curable paste connected to a semiconductor element, a sinterable paste, a manufacturing process and a use. The disclosed method produces a chip with an aluminum-silicon-copper surface metal of 5 micrometers thickness. The bonding copper sheet is oxygen-free copper, and due to process limitations, a thickness of 50 micrometers is selected. The package type is TO247.
[0108] Examples 1-3 yielded finished chips with copper bumps (copper material grade EFTET64, thickness 100 micrometers), bonding copper sheet thickness 10 mm, and package type TO247.
[0109] After packaging the chips fabricated using the processes of Examples 1-3, as well as the chips fabricated using conventional methods and Comparative Example 1, the following tests were performed:
[0110] Thermal conductivity test method: based on the International Electrotechnical Commission test standard JESD51.
[0111] Reliability testing method: Refer to the Automotive Electronics Committee Discrete Device Testing Standard AEC-Q101.
[0112] The test results are shown in Table 1.
[0113] Table 1
[0114]
[0115] The test results in Table 1 show that the current carrying capacity and heat dissipation capacity of the single chip obtained in Examples 1-3 of the present invention are superior to those of the traditional method and Comparative Example 1.
[0116] Finally, it should be noted that the above specific embodiments are only used to illustrate the technical solutions of the present invention and not to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention, and all such modifications or substitutions should be covered within the scope of the claims of the present invention.
Claims
1. A process for fabricating a wafer and metal bump bonding structure, comprising: The process includes the following steps: Step S1: Provide a metal sheet (9) and a wafer (4); Step S2: Attach a support film (2) to one side of the metal sheet (9), chemically etch a sintering surface on the other side of the metal sheet (9), form a support frame (1) on the outer periphery of the sintering surface, and form a plurality of spaced metal bumps (3) in the support frame (1) of the sintering surface. Clean the surface to obtain metal bumps (3) with support frame (1) and support film (2). Step S3: A paste layer (5) is formed on the wire bonding area of the wafer (4), and one side of the metal bump (3) is placed on the paste layer (5); or a dry paste film (6) is formed on the sintering surface of the metal bump (3), and one side of the dry paste film (6) is placed on the wire bonding area of the wafer (4). Step S4: Sinter the metal bump (3) from step S3 with the wafer (4), and remove the support film and support frame (1) to obtain a wafer-metal bump bonding structure; Step S5: Cut and separate the bonding structure from step S4 into individual chips.
2. The wafer and metal bump bonding structure fabrication process of claim 1, wherein, In step S1, the metal sheet (9) is made of one of copper, copper-molybdenum alloy, or tungsten-copper alloy, and the thickness of the metal sheet (9) is 50-300 micrometers. Step S2 also includes: electroplating silver on the sintering surface of the metal sheet (9) to form a sintering surface with a silver layer, wherein the thickness of the silver layer is 1-4 micrometers.
3. The method of claim 1, wherein the metal bump is formed by a process comprising: Step S3 involves fabricating a paste layer (5) on the wire bonding area of the wafer (4) and placing one side of the metal bump (3) on the paste layer (5). Specifically, this includes the following steps: Step S31: Mix the metal particles, solvent and sintering accelerator to obtain a wet slurry; Step S32: Apply a layer of wet paste to the wire bonding area of the wafer (4) by screen printing or dispensing to form a paste layer (5) with a thickness of 10-200 micrometers. Step S33: Place one side of the metal bump (3) on the slurry layer (5).
4. The wafer and metal bump bonding structure fabrication process of claim 3, wherein, Step S4 specifically includes the following steps: The metal bump (3) and the wafer (4) from step S3 are transferred to an oxygen-free oven, filled with nitrogen, and the oxygen content is controlled to be below 50 ppm. The temperature is raised to 150°C within 0.5 h and held for 0.5 h. Then the temperature is raised to 220°C within 0.5 h and held for 1 h. After that, the support film (2) and the support frame (1) are removed at 220°C to obtain the wafer-metal bump bonding structure.
5. The fabrication process of the wafer-metal bump bonding structure as described in claim 1, characterized in that, Step S3 involves fabricating a paste layer (5) on the wire bonding area of the wafer (4) and placing one side of the metal bump (3) on the paste layer (5). Specifically, this includes the following steps: Step S31: Mix the metal particles, solvent and sintering accelerator to obtain a wet slurry; Step S32: Apply a layer of wet paste to the wire bonding area of the wafer (4) by screen printing or dispensing to form a paste layer (5) with a thickness of 10-200 micrometers. Step S33: Transfer the wafer (4) coated with slurry layer (5) to an oxygen-free oven, fill it with nitrogen, control the oxygen content to be less than 50 ppm, raise the temperature to 150°C within 0.5 h and keep it for 1 h to obtain a semi-cured slurry layer (5). Step S34: Place one side of the metal bump (3) on the semi-cured slurry layer (5).
6. The process of claim 1, wherein the process further comprises: Step S3 involves forming a dry paste film (6) on the sintering surface of the metal bump (3) and placing one side of the dry paste film (6) on the wire bonding area of the wafer (4). Specifically, this includes the following steps: Step S31: Mix the metal particles, solvent and sintering accelerator to obtain a wet slurry; Step S32: Transfer the wet paste onto the support film (7) using a screen printing process; Step S33: Transfer the wet slurry and the supporting film (7) into the oven, raise the temperature to 100-150℃ in 0.5h, maintain it for 1-3h, and obtain the dry slurry film (6). Step S34: The dry slurry film (6) is bonded to the side of the metal bump (3) with the sintered surface by pressure transfer. Step S35: Place one side of the dry slurry film (6) on the wire bonding area of the wafer (3).
7. The wafer and metal bump bonding structure fabrication process of any one of claims 3, 5, 6, wherein, In step S31, the metal particles are selected from silver particles or copper particles, the particle size of the metal particles is 50nm-100nm, the solvent is an alcohol or ether organic compound with a carbon chain of 4 to 8, and the sintering promoter is an aliphatic amine.
8. The wafer and metal bump bonding structure fabrication process of any one of claims 5, 6, wherein, Step S4 specifically includes: The metal bump (3) and the wafer (4) from step S3 are transferred together and pressure sintering fixtures are transferred to a pressure sintering machine for sintering. Then the support film (2) and the support frame (1) are removed to obtain a wafer-metal bump bonding structure. The sintering temperature is 230-280℃, the sintering time is 150-250 seconds, the sintering pressure is 8-20 MPa, and the temperature at which the support film is removed is 220℃.
9. The process of claim 1, wherein the process further comprises: 5 applying a photoresist layer on the wafer; and exposing the photoresist layer to a light source to form a photoresist pattern on the wafer. 10 Step S4 is followed by a molding step, which is as follows: the gap between the wafer (4) and the metal bump (3) in the bonding structure is filled with epoxy resin and then molded with a transfer film to obtain a transfer-molded bonding structure. The molding temperature is 110-150℃ and the molding time is 50-150s.
10. A wafer and metal bump bonding structure, comprising: It is manufactured using the manufacturing process described in any one of claims 1-9.