Sacrificial layer prepreg for composite material and preparation method therefor
By developing a method for preparing sacrificial layer prepreg for composite materials, the problem of non-reusability caused by over-milling of tooling was solved, enabling flexible adjustment of tooling thickness and improvement of chemical corrosion resistance, and simplifying the processing.
Patent Information
- Application Number
- PCT/CN2025/133710
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-14
- Filing Date
- 2025-11-10
- Publication Date
- 2026-11-19
AI Technical Summary
In the existing composite material molding process, the problem of tooling over-milling leads to the inability to be reused, which affects the quality and cost of the tooling.
The method for preparing sacrificial layer prepreg for composite materials involves mixing inorganic fillers with resin to form a film, coating it onto the fiber surface to form a sacrificial layer prepreg, and then co-curing it with microwave absorbing prepreg and structural prepreg to achieve tooling thickening and composite material molding. The sacrificial layer can be manually peeled off later.
It enables flexible adjustment and precise control of tooling thickness, avoids tooling scrap, improves tooling life and chemical corrosion resistance of composite materials, and simplifies the processing.
Smart Images

Figure CN2025133710_19112026_PF_FP_ABST
Abstract
Description
A sacrificial layer prepreg for composite materials and its preparation method Technical Field
[0001] This application belongs to the field of composite material molding technology, specifically relating to a sacrificial layer prepreg for composite materials and its preparation method. Background Technology
[0002] Composite material processing equipment (referred to as composite process equipment or composite tooling) is used for molding composite material parts for aerospace airframes, mainly employing autoclave molding, resin transfer molding (RTM), and compression molding. Among these, autoclave molding is widely used in layup tooling (LM) for large composite panel construction. Composite materials differ significantly from metallic materials; the molding of composite materials and the molding of structural components are completed simultaneously. The structural properties of composite materials are highly sensitive to the manufacturing process and the structure of the composite tooling. The final properties of the material are also imparted through the tooling and manufacturing process. The manufacturing process and tooling structure directly affect the quality of composite structural components. If any aspect of the process or composite tooling is unreasonable, it can lead to manufacturing defects and dimensional deviations in the composite material, severely affecting its performance and even causing component scrapping, such as over-milling.
[0003] Over-milling refers to the phenomenon where, during milling, the cutting depth of the milling cutter exceeds the predetermined value or the milling time is too long, resulting in excessive cutting. This phenomenon negatively impacts the quality of the workpiece. Furthermore, scrapping affected tooling and remanufacturing it incurs extremely high tooling costs. Therefore, if over-milling occurs during actual composite forming, the tooling needs to be thickened. Similarly, in actual composite forming, there are also situations where design requirements necessitate thickening the tooling.
[0004] Therefore, there is an urgent need for a method that allows for free adjustment of tooling thickness, which can be used to thicken the tooling during the composite molding process. Summary of the Invention
[0005] The purpose of this application is to provide a sacrificial layer prepreg for composite materials and its preparation method, which can solve the problem that the tooling becomes too thin after milling to be reused.
[0006] To achieve the above objectives, this application provides a method for preparing a sacrificial layer prepreg for composite materials, comprising the following steps:
[0007] Inorganic fillers are mixed with resin and then subjected to film formation treatment to obtain resin film;
[0008] The resin film is coated onto the surface of the fiber to obtain a sacrificial layer prepreg;
[0009] After the sacrificial layer prepreg is prepared, according to the tooling thickness requirements, the sacrificial layer prepreg, microwave absorbing prepreg, and structural prepreg are sequentially laid on the tooling surface. Co-curing and demolding are then performed according to the curing process of the structural prepreg to obtain a composite material with a surface coated with the sacrificial layer prepreg; wherein:
[0010] The fiber is an aramid unidirectional tape or an aramid fabric.
[0011] Furthermore, the inorganic filler is an inorganic rigid particle, and the filling amount of the inorganic filler in the resin film is 10wt%~90wt%.
[0012] Furthermore, the inorganic filler includes at least one of alumina, glass microspheres, and silica, and the resin includes at least one of epoxy resin, bismaleimide resin, and cyanate ester resin.
[0013] Furthermore, the basis weight of the resin film is 10 g / m³. 2 ~200g / m 2 .
[0014] Furthermore, the fiber is an aramid unidirectional tape or aramid fabric, and the mass ratio of inorganic filler to fiber in the sacrificial layer prepreg is (1~2):10.
[0015] Furthermore, the microwave absorbing prepreg is composed of microwave absorbing resin and fiber carrier, and the fiber carrier content in the microwave absorbing prepreg is 30wt%~90wt%; the raw materials of the microwave absorbing resin include metal absorber and resin, and the metal absorber content in the microwave absorbing resin is 40wt%~98wt%.
[0016] Furthermore, the structural prepreg is made by combining resin and carbon fiber, and the carbon fiber content in the structural prepreg is 60wt%~70wt%.
[0017] Furthermore, the step of laying the sacrificial prepreg on the tooling surface includes laying at least one layer of the sacrificial prepreg, with a thickness of 0.1mm to 10mm after laying.
[0018] Furthermore, the curing process includes the following steps:
[0019] The autoclave curing method is used to increase the internal pressure of the autoclave to 3 bar to 6 bar, raise the temperature to 120°C to 180°C and keep it constant for 30 min to 240 min; continue to raise the temperature to 190°C to 260°C and keep it constant for 30 min to 240 min; lower the temperature to 30°C to 80°C and depressurize.
[0020] This application also provides a sacrificial layer prepreg for composite materials, which is prepared using the above-described preparation method.
[0021] In summary, this application has the following advantages:
[0022] The sacrificial prepreg for composite materials prepared in this application possesses excellent tooling adaptability and convenience. After being laid on the tooling surface, the tooling thickness can be flexibly adjusted according to specific tooling design requirements, enabling rapid and simple tooling preparation. The sacrificial prepreg on the composite material surface can be removed through a simple tearing operation, simultaneously achieving tooling thickening and composite molding during the composite molding process. Furthermore, the residual resin film forms a protective layer on the composite material surface, significantly improving the composite material's chemical corrosion resistance and extending the tooling's service life.
[0023] Specifically, in this application, the sacrificial prepreg mainly serves as a tooling thickening structure. The thickness of the tooling thickening is calibrated by the coating thickness of the sacrificial prepreg. It can be layered and laid according to the tooling size and shape requirements to achieve precise control of the tooling thickness. In this application, the microwave absorbing prepreg mainly serves as a microwave absorbing functional layer to provide microwave absorbing performance for the composite material. In this application, the structural prepreg undertakes the main mechanical properties of the composite material (such as strength, stiffness, etc.). That is, the microwave absorbing prepreg and the structural prepreg in this application form a composite material. The sacrificial prepreg in this application is used to thicken the tooling during the composite material molding process, and it can be removed from the surface of the composite material after molding without affecting the structure of the original tooling or the structure of the composite material. Attached Figure Description
[0024] Figure 1 is a comparison of the sacrificial layer prepreg for composite materials prepared in Example 1 of this application after manual tearing; wherein, Figure 1(a) is a photo of the sacrificial layer prepreg for composite materials before tearing, Figure 1(b) is a photo of the sacrificial layer prepreg for composite materials during the tearing process, and Figure 1(c) is a photo of the prepreg for composite materials after tearing.
[0025] Figure 2 shows the results of the salt spray test on the composite materials prepared in Example 1 and Comparative Example 1 of this application. Embodiments of the present invention
[0026] Composite materials are composed of two or more different materials, possessing characteristics such as lightweight, high strength, corrosion resistance, and good damping properties, and are widely used in aviation, aerospace, and automotive fields. To produce composite material products, corresponding tooling and equipment need to be designed to achieve the molding, joining, and assembly of composite materials. The development of composite materials is of great significance to improving the performance of aviation equipment; the performance of an aircraft depends half on its design and the other half on the materials used. Due to their unique physical and chemical properties, composite materials have a profound impact on the speed, altitude, range, and maneuverability of aircraft. Composite materials are widely used in the aviation field for military aircraft, civilian aircraft, helicopters, drones, aero engines, and other defense industries; currently, the vast majority of structural components in aircraft are made of composite materials.
[0027] Composite molding tooling refers to tooling equipment designed for manufacturing composite molded products. It consists of tools and equipment used in the composite material manufacturing process for molding and assembling composite materials. Its main function is to ensure that the shape, size, and performance of composite material components meet design requirements, while improving production efficiency and reducing costs. In the aerospace field, composite tooling is mainly used to manufacture critical parts of rockets, aircraft, and other aircraft, such as wings and fuselages. Therefore, tooling design needs to meet the requirements of high precision and high strength.
[0028] In composite forming tooling technology, milling is typically required for the following reasons: ① Excess material or burrs remaining on the tooling die affect the tooling's accuracy and surface quality; ② To adjust the tooling's size and shape and correct dimensional errors; ③ To improve the tooling's surface quality and reduce surface roughness; ④ To machine various complex shapes to meet the needs of tooling with different shapes and sizes. However, in actual milling processes, cutting forces can cause localized machining deformation and tool deflection in the parts, leading to localized machining deformation and irreversible plastic deformation. Simultaneously, high material removal rates and complex cross-sectional shapes during high-speed cutting can cause the release and rebalancing of residual stress, also resulting in workpiece deformation. These deformations can lead to over-milling of the tooling, causing it to become thinner and unusable, ultimately rendering it scrap.
[0029] Therefore, this application proposes a method for preparing a sacrificial layer prepreg for composite materials. The prepared sacrificial layer prepreg comprises three different functional materials. Throughout the entire composite molding process (including the tooling thickening process and the composite material preparation process within the thickened tooling), the cured sacrificial layer prepreg primarily functions as a sacrificial layer. On one hand, it can directly thicken over-milled or insufficiently thick tooling; on the other hand, composite molding can be directly performed within the thickened tooling. After molding, the sacrificial layer is easily peeled off and will not negatively impact the molded composite material or the used tooling. The microwave-absorbing prepreg, after curing, serves as the microwave-absorbing functional layer of the composite material, while the structural prepreg, after curing, provides structural strength to the composite material. Based on this, the sacrificial layer of this application is very easy to peel off after molding on the tooling surface, and can play a supporting, isolating, and easily removable role in subsequent processing during the co-curing process.
[0030] The principles and features of this application are described below with reference to embodiments. The examples are for illustrative purposes only and are not intended to limit the scope of this application. Unless otherwise specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all commercially available conventional products.
[0031] This application provides a method for preparing a sacrificial layer prepreg for composite materials, comprising the following steps:
[0032] Inorganic fillers are mixed with resin and then subjected to film formation treatment to obtain resin film;
[0033] The resin film is coated onto the surface of the fiber to obtain a sacrificial layer prepreg;
[0034] After the sacrificial layer prepreg is prepared, according to the tooling thickness requirements, the sacrificial layer prepreg, microwave absorbing prepreg, and structural prepreg are sequentially laid on the tooling surface. Co-curing and demolding are then performed according to the curing process of the structural prepreg to obtain a composite material with a surface coated with the sacrificial layer prepreg; wherein:
[0035] The fiber is an aramid unidirectional tape or an aramid fabric.
[0036] In this application, the sacrificial layer prepreg is prepared by first mixing inorganic fillers with resin to form a resin film, which reduces the resin's adhesion and makes the sacrificial layer easier to peel off. Then, aramid fibers are used to provide flexible support, ensuring no breakage during subsequent tearing. In the composite structure, a microwave-absorbing prepreg imparts functional properties to the composite material (e.g., microwave-absorbing resin provides stealth capabilities), and a structural prepreg provides structural strength. Co-curing of the three prepregs ensures perfect interface bonding, and the use of the structural prepreg's curing process for co-curing avoids delamination or incomplete curing, thus achieving thickening and molding. Using the above method, a composite material with a surface coated with a sacrificial layer prepreg can be obtained. The sacrificial layer formed by the prepreg on the surface of this composite material is easily peeled off without affecting other structures of the composite material. Simultaneously, the tooling component after demolding will not undergo any structural changes and can be reused (this reuse indicates both that the tooling component can be reused without any further treatment and that other composite material molding requirements can be met by applying the same sacrificial layer prepreg coating to the tooling component).
[0037] In this application, aramid fibers are combined with a resin film containing inorganic fillers, solving the problem that traditional thickening methods cannot simultaneously achieve easy peeling and precise thickness control. Through the co-curing of sacrificial prepreg, microwave-absorbing prepreg, and structural prepreg, functional integration (such as microwave absorption + structural reinforcement) and interface compatibility are achieved, avoiding the defects of traditional delamination processes. The composite material prepared by this method can be manually torn for processing, improving peeling efficiency. The sacrificial prepreg in this application is mainly used for tooling thickening and provides sacrificial points in the later stages. The microwave-absorbing prepreg is used to impart new functions to the molded composite material (i.e., the material after co-curing and demolding treatment, which separates the original tooling from the molded composite material). The structural prepreg mainly provides structural strength to the composite material. After subsequent curing and demolding, a composite material with a sacrificial layer covering the surface can be obtained. The final composite material can then be obtained by tearing the cured section of the sacrificial prepreg.
[0038] In this application, after stripping the aramid fibers closest to the composite material, a resin film remains on the surface of the composite material. This residual resin film can improve the corrosion resistance of the composite material and also provide a substrate with high adhesion for subsequent spraying. The preparation method of this application can also avoid tooling scrapping, improve the tooling life and reuse rate, and solve the long-standing problem of tooling thickening in the industry.
[0039] In some optional embodiments of this application, the inorganic filler is a rigid inorganic particle, and the filling amount of the inorganic filler in the resin film is 10wt%~90wt%. The inorganic filler in this application can reduce the adhesion of the resin, making the sacrificial layer easier to peel off. Furthermore, the presence of the inorganic filler can reduce the fluidity of the resin, further ensuring film-forming performance. Simultaneously, the content of the inorganic filler needs to balance peelability and film strength. If the inorganic filler content is too low (<10wt%), it will result in excessive adhesion, making peeling difficult. If the inorganic filler content is too high (>90wt%), it will cause the resin film to become brittle, thus preventing film formation.
[0040] In some optional embodiments of this application, the inorganic filler includes at least one of alumina, glass microspheres, and silica, and the resin includes at least one of epoxy resin, bismaleimide resin, and cyanate ester resin. The inorganic filler can reduce the adhesion between the sacrificial layer prepreg and the resin, making the sacrificial layer easier to peel off. The selection of the resin system maintains consistency with the resin system in the microwave absorbing prepreg and the structural prepreg, meeting the requirements of the co-curing process. For example, when the resin used in the sacrificial layer prepreg is epoxy resin, the resin in the microwave absorbing prepreg and the structural prepreg is also epoxy resin; for example, when the resin used in the sacrificial layer prepreg is bismaleimide resin, the resin in the microwave absorbing prepreg and the structural prepreg is also bismaleimide resin. This application preferably uses a high-temperature epoxy resin.
[0041] In some optional embodiments of this application, the basis weight of the resin film is 10 g / m³. 2 ~200g / m 2 An appropriate basis weight of the resin film is necessary to ensure the composite material meets non-destructive quality standards while avoiding excessively high basis weight, which could lead to increased peeling force and difficulty in peeling. However, if the basis weight of the resin film is too low, i.e., the resin film is too thin, a continuous film layer cannot be formed, resulting in an incomplete protective layer and poor corrosion resistance. It is worth noting that in the final composite material prepared in this application, the resin film containing inorganic fillers remaining on the surface after peeling forms a protective layer, and no rust was observed after 7 days of salt spray testing. Simultaneously, the residual resin film provides a rough interface to the composite material surface, improving surface adhesion.
[0042] In some optional embodiments of this application, the fiber is an aramid unidirectional tape or aramid fabric, and the mass ratio of inorganic filler to fiber in the sacrificial layer prepreg is (1~2):10. In this application, aramid fiber is used as the carrier; its flexibility allows the sacrificial layer to be manually torn off, replacing traditional glass fiber (glass fiber is brittle and can only be CNC milled). The mass ratio of inorganic filler to fiber ensures a balance between the fiber's load-bearing capacity and the resin filling. If the fiber ratio is too low (e.g., the mass ratio of inorganic filler to fiber < 1:10), the resin film thickness will be large, leading to difficulty in peeling; if the fiber ratio is too high (e.g., the mass ratio of inorganic filler to fiber > 2:10), the sacrificial layer will lack rigidity and be prone to tearing.
[0043] In some optional embodiments of this application, the microwave absorbing prepreg is composed of a microwave absorbing resin and a fiber carrier, wherein the fiber carrier content in the microwave absorbing prepreg is 30wt%~90wt%; the raw materials of the microwave absorbing resin include at least a metal absorber and resin, wherein the metal absorber content in the microwave absorbing resin is 40wt%~98wt%. The microwave absorbing prepreg produces a microwave absorbing layer, which can impart stealth properties to the composite material. The metal absorber includes ferrite, carbonyl iron powder, or silicon carbide, and the particle size of the metal absorber is 1μm~10μm.
[0044] Specifically, the microwave absorbing prepreg of this application can be prepared by a hot-melt method, including:
[0045] Metal absorber and resin were mixed at a specific mass ratio and heated to 80°C. The mixture was then stirred evenly using a high-speed stirring device (60-120 rpm) to obtain the microwave absorbing resin. The resin was then melted on an 80°C hot plate and prepared using a two-roll mill to a weight of 300 g / m³. 2 The microwave absorbing resin film is prepared by placing two layers of microwave absorbing resin film on both sides of a fiber carrier and hot pressing them at 45°C.
[0046] In some optional embodiments of this application, the structural prepreg is composed of resin and carbon fiber, and the carbon fiber content in the structural prepreg is 60wt%~70wt%. The structural prepreg is used to prepare a structural layer, which can provide structural strength for the composite material.
[0047] Specifically, the structural prepreg is prepared by the following method:
[0048] The resin was melted on an 80°C hot plate and prepared using a two-roll mill to a basis weight of 62 g / m³. 2 The resin film is prepared by placing two layers of resin film on both sides of a layer of carbon fiber and hot pressing them at 45°C to obtain a structural prepreg.
[0049] In some optional embodiments of this application, a sacrificial prepreg is laid on the surface of the tooling, including laying at least one layer of the sacrificial prepreg, with a thickness of 0.1 mm to 10 mm after laying. The laying thickness determines the thickness of the tooling thickening, so the thickness of the sacrificial prepreg laying can be determined according to the need for tooling thickening.
[0050] The preparation method of this application can adjust the thickness of the tooling (for example, the thickness after laying one layer of sacrificial prepreg is 0.1 mm, and two layers are 0.2 mm). By adjusting the number of sacrificial prepreg layers, the tooling thickness requirement can be precisely controlled, avoiding the errors caused by traditional CNC milling, reducing time consumption, and improving processing efficiency and accuracy.
[0051] Furthermore, the curing process includes the following steps:
[0052] The autoclave curing method is used to increase the internal pressure of the autoclave to 3 bar to 6 bar, raise the temperature to 120°C to 180°C and keep it constant for 30 min to 240 min; continue to raise the temperature to 190°C to 260°C and keep it constant for 30 min to 240 min; lower the temperature to 30°C to 80°C and depressurize.
[0053] Secondly, based on a general inventive concept, this application also provides a sacrificial layer prepreg for composite materials, prepared using the above-described preparation method. After curing and demolding the sacrificial layer prepreg for composite materials, a composite material with the surface coated with the sacrificial layer prepreg can be obtained. By picking up and manually tearing off the single-layer fibers in the sacrificial layer structure formed by the sacrificial layer prepreg, a resin film can be retained on the surface of the composite material. The retained resin film can improve the chemical corrosion resistance of the molded composite material.
[0054] As a further improvement to this application, a corresponding functional coating can be sprayed onto the surface of this composite material to achieve functions such as stealth, thermal protection, electrical conductivity, and thermal conductivity.
[0055] The method provided in this application differs from the traditional method of directly thickening the tooling. It uses a sacrificial layer prepreg to thicken the tooling, which can achieve the purpose of freely adjusting the thickness. It can also impart a certain degree of chemical corrosion resistance to the surface of the composite material after the sacrificial layer prepreg is peeled off.
[0056] The technical solutions described above in this application will be explained in detail below with reference to specific embodiments.
[0057] Example 1
[0058] This embodiment provides a method for preparing a sacrificial layer prepreg for composite materials, which requires increasing the tooling thickness by 0.2 mm, and includes the following steps:
[0059] (1) Add silica to epoxy resin and perform film formation treatment to obtain a basis weight of 40 g / m 2 The resin film contains 80% silica by mass.
[0060] (2) Coat the two layers of resin film onto a surface with a density of 100 g / m². 2 Aramid fabric surface is hot-pressed at 45°C to obtain sacrificial layer prepreg;
[0061] (3) The sacrificial prepreg is laid on the surface of the tooling to obtain the first sacrificial layer with a single layer thickness of 0.1 mm;
[0062] (4) Then lay the sacrificial prepreg on the surface of the first sacrificial layer to obtain a total sacrificial layer with a total thickness of 0.2 mm;
[0063] (5) Preparation of microwave absorbing prepreg: Carbonyl iron powder with a particle size of 5 μm and epoxy resin were mixed at a mass ratio of 72:28 and heated to 80°C. The mixture was then stirred evenly using a high-speed stirring device (120 r / min) to obtain microwave absorbing resin. The microwave absorbing resin was melted on an 80°C hot plate and prepared using a double roller to a weight of 300 g / m³. 2 The microwave absorbing resin film is prepared by coating two layers of microwave absorbing resin film onto the surface of a layer of carbon fiber and hot pressing them at 45°C to obtain microwave absorbing prepreg.
[0064] (6) Preparation of structural prepreg: The epoxy resin is melted on an 80°C hot plate and prepared into a prepreg with a basis weight of 62 g / m³ using a two-roller press. 2 The resin film is prepared by placing two layers of resin film on both sides of a layer of carbon fiber and hot pressing them at 45°C to obtain a structural prepreg.
[0065] (7) Continue to lay and stack 4 layers of microwave absorbing prepreg and 10 layers of structural prepreg on the surface of the total sacrificial layer, and co-cur according to the curing process parameters of the structural prepreg. After completion, demold. The curing process includes: using an autoclave for curing, pressurizing the inside of the autoclave to 5 bar, raising the temperature to 135°C, and holding it at that temperature for 60 min; continuing to raise the temperature to 160°C and holding it at that temperature for 120 min; finally, cooling the temperature to 60°C and then depressurizing and removing the vacuum from the autoclave (this curing process is used in the following examples and comparative examples).
[0066] As shown in Figure 1, after demolding, the final composite material can be obtained by tearing along the aramid fabric in the second sacrificial layer. In Figure 1, Figure 1(a) is a photo of the prepreg of the sacrificial layer for the composite material before tearing, Figure 1(b) is a photo of the prepreg of the sacrificial layer for the composite material during the tearing process, and Figure 1(c) is a photo of the composite material after tearing.
[0067] An infrared absorbing coating was directly sprayed onto the surface of the composite material. The composite material was then subjected to a salt spray test using 5wt% sodium chloride. After seven days, it was removed, and as shown in Figure 2, no yellow rust marks were observed on the surface, indicating that the resin film remaining on the surface of the composite material can significantly improve its chemical corrosion resistance. The adhesion of the molded composite material surface was measured to be 28 MPa (room temperature, test standard GB / T5210) using an adhesion tester.
[0068] Example 2
[0069] This embodiment provides a method for preparing a sacrificial layer prepreg for composite materials, requiring a 0.8 mm thickening of the same tooling as in Example 1, including the following steps:
[0070] (1) Add silica to epoxy resin and perform film formation treatment to obtain a basis weight of 40 g / m 2 The resin film contains 80% silica by mass.
[0071] (2) Coat the two layers of resin film onto a surface with a density of 100 g / m². 2 A sacrificial layer prepreg is obtained by laminating the surface of aramid fabric;
[0072] (3) The sacrificial prepreg is laid on the surface of the tooling to obtain the first sacrificial layer with a single layer thickness of 0.1 mm;
[0073] (4) Continue to lay the sacrificial prepreg on the surface of the first sacrificial layer to obtain a total sacrificial layer with a total thickness of 0.8 mm;
[0074] (5) Preparation of microwave absorbing prepreg: Carbonyl iron powder with a particle size of 5 μm and epoxy resin were mixed at a mass ratio of 72:28 and heated to 80°C. The mixture was then stirred evenly using a high-speed stirring device (120 r / min) to obtain microwave absorbing resin. The microwave absorbing resin was melted on an 80°C hot plate and prepared using a double roller to a weight of 300 g / m³. 2 The microwave absorbing resin film is prepared by coating two layers of microwave absorbing resin film onto both sides of a layer of carbon fiber and hot pressing them at 45°C to obtain microwave absorbing prepreg.
[0075] (6) Preparation of structural prepreg: The epoxy resin is melted on an 80°C hot plate and prepared into a prepreg with a basis weight of 62 g / m³ using a two-roller press. 2 The resin film is prepared by placing two layers of resin film on both sides of a layer of carbon fiber and hot pressing them at 45°C to obtain a structural prepreg.
[0076] (7) Continue to lay and stack 4 layers of microwave absorbing prepreg and 10 layers of structural prepreg on the surface of the total sacrificial layer, and co-cur them according to the structural prepreg curing process parameters of Example 1. After completion, demold.
[0077] After demolding, the aramid fabric in the 8th sacrificial layer is torn to obtain the final molded composite material. The molded composite material is placed in a 5wt% sodium chloride salt spray test. After seven days, it is removed and observed that there are no yellow rust marks on its surface.
[0078] Example 3
[0079] This embodiment provides a method for preparing a sacrificial layer prepreg for composite materials, requiring a 0.2 mm thickening of the same tooling as in Example 1, including the following steps:
[0080] (1) Add silica to epoxy resin and perform film formation treatment to obtain a basis weight of 40 g / m 2 The resin film contains 80% silica by mass.
[0081] (2) Coat the two layers of resin film onto a surface with a density of 100 g / m². 2 A unidirectional aramid tape surface is composited to obtain a sacrificial layer prepreg;
[0082] (3) The sacrificial prepreg is laid on the surface of the tooling to obtain the first sacrificial layer with a single layer thickness of 0.1 mm;
[0083] (4) Then lay the sacrificial prepreg on the surface of the first sacrificial layer to obtain a total sacrificial layer with a total thickness of 0.2 mm;
[0084] (5) Preparation of microwave absorbing prepreg: Carbonyl iron powder with a particle size of 5 μm and epoxy resin were mixed at a mass ratio of 72:28 and heated to 80°C. The mixture was then stirred evenly using a high-speed stirring device (120 r / min) to obtain microwave absorbing resin. The microwave absorbing resin was melted on an 80°C hot plate and prepared using a double roller to a weight of 300 g / m³. 2 The microwave absorbing resin film is prepared by coating two layers of microwave absorbing resin film onto both sides of a layer of carbon fiber and hot pressing them at 45°C to obtain microwave absorbing prepreg.
[0085] (6) Preparation of structural prepreg: The epoxy resin is melted on an 80°C hot plate and prepared into a prepreg with a basis weight of 62 g / m³ using a two-roller press. 2 The resin film is prepared by placing two layers of resin film on both sides of a layer of carbon fiber and hot pressing them at 45°C to obtain a structural prepreg.
[0086] (7) Continue to lay and stack 4 layers of microwave absorbing prepreg and 10 layers of structural prepreg on the surface of the total sacrificial layer, and co-cur them according to the structural prepreg curing process parameters of Example 1. After completion, demold.
[0087] After demolding, the final molded composite material can be obtained by tearing along the aramid unidirectional tape in the second sacrificial layer. The molded composite material was placed in a 5wt% sodium chloride salt spray test. After seven days, it was removed and observed that there were no yellow rust marks on its surface.
[0088] Comparative Example 1
[0089] This comparative example provides a method for preparing a sacrificial layer prepreg for composite materials, the method comprising the following steps:
[0090] (1) Preparation of microwave absorbing prepreg: Carbonyl iron powder with a particle size of 5 μm and epoxy resin were mixed at a mass ratio of 72:28 and heated to 80°C. The mixture was then stirred evenly using a high-speed stirring device (speed 120 r / min) to obtain microwave absorbing resin. The microwave absorbing resin was melted on an 80°C hot plate and prepared using a double roller to a weight of 300 g / m³. 2 The microwave absorbing resin film is prepared by coating two layers of microwave absorbing resin film onto both sides of a layer of carbon fiber and hot pressing them at 45°C to obtain microwave absorbing prepreg.
[0091] (2) Preparation of structural prepreg: The epoxy resin was melted on an 80°C hot plate and prepared into a prepreg with a basis weight of 62 g / m³ using a two-roller press. 2 The resin film is prepared by placing two layers of resin film on both sides of a layer of carbon fiber and hot pressing them at 45°C to obtain a structural prepreg.
[0092] (3) Lay two layers of microwave absorbing prepreg and 10 layers of structural prepreg on the surface of the tooling in sequence, and co-cur according to the curing process parameters of the structural prepreg, and demold after completion.
[0093] The composite material obtained after demolding was placed in a 5wt% sodium chloride salt spray test. After seven days, it was taken out. As shown in Figure 2, it can be seen that the surface of the composite material without the preparation of the sacrificial layer prepreg has yellow rust marks.
[0094] Comparative Example 2
[0095] This comparative example provides a method for preparing a sacrificial layer prepreg for composite materials, requiring a 0.2 mm thickening of the same tooling as in Example 1. The preparation method includes the following steps:
[0096] (1) Add silica to epoxy resin and perform film formation treatment to obtain a basis weight of 40 g / m 2 The resin film contains 80% silica by mass.
[0097] (2) Coat the two layers of resin film onto a surface with a density of 100 g / m². 2 A glass fiber prepreg is obtained by laminating the surface of a glass fiber fabric.
[0098] (3) The glass fiber prepreg is laid on the surface of the tooling to obtain the first sacrificial layer with a single layer thickness of 0.1 mm;
[0099] (4) Then lay glass fiber prepreg on the surface of the first sacrificial layer to obtain a total sacrificial layer with a total thickness of 0.2 mm;
[0100] (5) Preparation of microwave absorbing prepreg: Carbonyl iron powder with a particle size of 5 μm and epoxy resin were mixed at a mass ratio of 72:28 and heated to 80°C. The mixture was then stirred evenly using a high-speed stirring device (120 r / min) to obtain microwave absorbing resin. The microwave absorbing resin was melted on an 80°C hot plate and prepared using a double roller to a weight of 300 g / m³. 2 The microwave absorbing resin film is prepared by coating two layers of microwave absorbing resin film onto both sides of a layer of carbon fiber and hot pressing them at 45°C to obtain microwave absorbing prepreg.
[0101] (6) Preparation of structural prepreg: The epoxy resin is melted on an 80°C hot plate and prepared into a prepreg with a basis weight of 62 g / m³ using a two-roller press. 2 The resin film is prepared by placing two layers of resin film on both sides of a layer of carbon fiber and hot pressing them at 45°C to obtain a structural prepreg.
[0102] (7) Continue to lay and stack 4 layers of microwave absorbing prepreg and 10 layers of structural prepreg on the surface of the total sacrificial layer, and co-cur them according to the structural prepreg curing process parameters of Example 1. After completion, demold.
[0103] After demolding, attempts were made to tear the glass fiber fabric along the second sacrificial layer, but it could not be removed by peeling, thus failing to obtain the final composite material. This is because glass fibers are brittle and cannot be removed by tearing; they can only be removed by CNC milling. Therefore, a CNC milling machine was used to cut 0.2 mm to obtain the final composite material. This composite material was then placed in a 5wt% sodium chloride salt spray test. After seven days, it was removed, and yellow rust marks were observed on its surface.
[0104] An infrared absorbing coating was directly sprayed onto the surface of the composite material obtained in Comparative Example 2 (without salt spray test), and the surface adhesion was measured to be 19 MPa using an adhesion tester.
[0105] As can be seen from Examples 1-3, the composite material prepared by the preparation method provided in this application, after demolding, allows for easy removal of the surface layer to be peeled off by manual tearing without affecting the structure and integrity of the composite material. A comparison between Example 1 and Comparative Example 1 shows that the final composite material prepared in this application still has a resin film remaining on the surface, which acts as a barrier and effectively prevents internal corrosion of the composite material. A comparison between Example 1 and Comparative Example 2 shows that the composite material with a sacrificial layer on the surface prepared in this application uses aramid fiber as a carrier during the preparation process. Therefore, the excellent flexibility of aramid fiber allows for manual tearing off of the sacrificial layer, resulting in excellent peeling performance without damaging the surface shape of the composite material itself. A comparison of surface adhesion tests between Example 1 and Comparative Example 2 shows that the preparation method provided in this application, compared to traditional CNC milling methods, can impart a rougher surface to the composite material, thereby improving surface adhesion. For example, the final composite material of this application has a rough surface (surface adhesion of 28 MPa), while the final composite material obtained by conventional processing has a smooth surface (surface adhesion of 19 MPa). Therefore, the preparation method of this application can significantly improve the adhesion of the surface sprayed material. That is, by spraying the corresponding functional coating on the surface, functions such as stealth, thermal protection, electrical conductivity and thermal conductivity can be achieved.
[0106] It is also worth mentioning that traditional processing methods usually remove the thickened part of the tooling by milling, but milling is difficult to remove the narrow area of the thickened tooling. The removal method of this application is simpler, not limited by the depth of the composite material and the narrow area, and is more flexible and controllable.
[0107] While specific embodiments of this application have been described in detail, this should not be construed as limiting the scope of protection of this application. Various modifications and variations that can be made by those skilled in the art without inventive effort within the scope described in the claims still fall within the scope of protection of this application.
Claims
1. A method for preparing a sacrificial layer prepreg for composites, characterized in that, Includes the following steps: Inorganic fillers are mixed with resin and then subjected to film formation treatment to obtain resin film; The resin film is coated onto the surface of the fiber to obtain a sacrificial layer prepreg; After the sacrificial layer prepreg is prepared, according to the tooling thickness requirements, the sacrificial layer prepreg, microwave absorbing prepreg, and structural prepreg are sequentially laid on the tooling surface. Co-curing and demolding are then performed according to the curing process of the structural prepreg to obtain a composite material with a surface coated with the sacrificial layer prepreg; wherein: The fiber is an aramid unidirectional tape or an aramid fabric.
2. The method of claim 1, wherein the method is characterized by: The inorganic filler is an inorganic rigid particle, and the filling amount of the inorganic filler in the resin film is 10wt%~90wt%.
3. The method for producing a sacrificial layer prepreg for composites according to claim 1 or 2, characterized in that, The inorganic filler includes at least one of alumina, glass microspheres, and silica, and the resin includes at least one of epoxy resin, bismaleimide resin, and cyanate ester resin.
4. The method of claim 1, wherein the method further comprises the step of: The resin adhesive film has a grammage of 10 g / m 2 ~200 g / m 2 .
5. The method of claim 1, wherein the method further comprises the step of: The mass ratio of inorganic filler to fiber in the sacrificial layer prepreg is (1~2):
10.
6. The method of claim 1, wherein the method further comprises the step of: The microwave absorbing prepreg is composed of microwave absorbing resin and fiber carrier, and the fiber carrier content in the microwave absorbing prepreg is 30wt%~90wt%; the raw materials of the microwave absorbing resin include metal absorber and resin, and the metal absorber content in the microwave absorbing resin is 40wt%~98wt%.
7. The method of claim 1, wherein the method further comprises the step of applying a sacrificial layer to the surface of the composite material. The structural prepreg is made by combining resin and carbon fiber, and the carbon fiber content in the structural prepreg is 60wt%~70wt%.
8. The method of claim 1, wherein the method further comprises the step of: The step of laying the sacrificial prepreg on the tooling surface includes laying at least one layer of the sacrificial prepreg, with a thickness of 0.1 mm to 10 mm after laying.
9. The method of claim 1, wherein the method further comprises the step of applying a sacrificial layer to the surface of the composite material. The curing process includes the following steps: The autoclave curing method is used to increase the internal pressure of the autoclave to 3 bar to 6 bar, raise the temperature to 120°C to 180°C and keep it constant for 30 min to 240 min; continue to raise the temperature to 190°C to 260°C and keep it constant for 30 min to 240 min; lower the temperature to 30°C to 80°C and depressurize.
10. A sacrificial layer prepreg for composites, characterized by, It is prepared by the method described in any one of claims 1-9.