Erasable organic-inorganic hybrid patterned thin film prepared by molecular layer deposition

By using molecular layer deposition technology to self-assemble organic-inorganic hybrid thin films on the substrate surface, the problems of film thickness uniformity, resolution and etching resistance of traditional photoresists in deep ultraviolet and extreme ultraviolet lithography processes are solved, enabling high-resolution patterning and reversible pattern erasure, and reducing costs.

WO2026237366A1PCT designated stage Publication Date: 2026-11-19EAST CHINA UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2025/143819
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-15
Filing Date
2025-12-19
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Traditional photoresists face challenges in deep ultraviolet and extreme ultraviolet lithography processes, including insufficient film thickness uniformity, limited resolution, weak etching resistance, and large line width roughness. Furthermore, the irreversibility after exposure leads to a high material waste rate, making it difficult to meet the requirements of sub-10nm nodes.

Method used

Inorganic metal precursors and organic ligands are alternately introduced using molecular layer deposition technology to form erasable organic-inorganic hybrid films on the substrate surface through self-assembly. By optimizing the precursor pulse time and cycle number, the film thickness and composition ratio can be precisely controlled, and the pattern can be reversibly erased by heating.

Benefits of technology

It improves the resolution, sensitivity, and etching resistance of photoresist, reduces costs, and has a high film surface flatness, enabling high-resolution patterning and reversible pattern erasure without a baking step.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2025143819_19112026_PF_FP_ABST
    Figure CN2025143819_19112026_PF_FP_ABST
Patent Text Reader

Abstract

An erasable organic-inorganic hybrid patterned thin film prepared by molecular layer deposition. By alternately depositing inorganic precursors and organic ligands, a high-precision and uniform hybrid photoresist thin film is formed on the surface of a substrate. The specific steps comprise: using MLD technology to precisely control the composition and thickness of a thin film by means of vacuum deposition, gas source switching and cyclic purging processes; using ultraviolet lithography or an electron beam to perform patterned exposure on the thin film; by means of heating and re-exposure, implementing pattern erasing and rewriting; and developing with a 0.01% oxalic acid solution. The obtained thin film has ultra-low roughness, high resolution and excellent etching resistance, and effectively solves the problems of uneven thickness, low sensitivity and high trial and error costs of conventional photoresist films; and in addition, the process flow is simplified, and the thin film is suitable for deep ultraviolet and extreme ultraviolet lithography processes.
Need to check novelty before this filing date? Find Prior Art

Description

Erasable organic-inorganic hybrid patterned thin films prepared by molecular layer deposition Technical Field

[0001] This invention relates to the field of semiconductor manufacturing materials technology, and more specifically to an erasable organic-inorganic hybrid patterned thin film prepared by molecular layer deposition. Background Technology

[0002] With the continuous improvement of semiconductor device integration, photolithography, as a core process in chip manufacturing, directly determines the performance and cost of integrated circuits through its precision and efficiency. Photoresist, a key material in photolithography, transfers mask patterns onto the silicon wafer surface through photochemical reactions, thereby forming nanoscale circuit structures. Traditional photoresists are mostly prepared using solution mixing methods, such as chemically amplified photoresist (CAR), which enhances sensitivity through photoacid catalysis. However, it still faces significant challenges in deep ultraviolet (DUV) and more advanced extreme ultraviolet (EUV) lithography processes: on the one hand, traditional methods have limited control over the molecular structure of photoresists, resulting in insufficient film thickness uniformity, limited resolution, and weak etching resistance during plasma etching; on the other hand, CAR relies on photoacid diffusion mechanisms, which easily leads to increased linewidth roughness (LWR), making it difficult to meet the requirements of sub-10nm nodes. More importantly, the exposure process of traditional photoresists is based on irreversible photochemical reactions (such as covalent bond breaking or cross-linking). Once exposure is complete, its molecular structure is permanently altered and cannot be restored to its initial state through physical or chemical means. This irreversibility means that exposure errors cannot be corrected, resulting in extremely high material waste, especially in complex mask verification or scientific research trial-and-error scenarios where costs are difficult to control.

[0003] This invention provides an erasable organic-inorganic hybrid patterned thin film prepared by molecular layer deposition (MLD). By alternately introducing inorganic metal precursors and organic ligands, an erasable patterned organic-inorganic hybrid thin film is self-assembled on a substrate surface. This method fully utilizes the self-limiting reaction characteristics of MLD technology to achieve precise control of film thickness and composition ratio. By optimizing the precursor pulse time and cycle number, the sensitivity and etching resistance of the film can be significantly improved, while avoiding the complex post-baking (PEB) step in traditional processes. In particular, this film can be patterned during exposure and the pattern can be erased by heating, demonstrating broad application prospects and research value. Summary of the Invention

[0004] The purpose of this invention is to provide an erasable organic-inorganic hybrid patterned thin film prepared by molecular layer deposition. This novel erasable organic-inorganic hybrid patterned thin film has potential application value in enhancing photoresist resolution and sensitivity, reducing roughness, and lowering costs.

[0005] The objective of this invention is achieved through the following technical solution:

[0006] An erasable organic-inorganic hybrid patterned thin film prepared by molecular layer deposition, wherein the molecular layer deposition preparation includes the following steps:

[0007] S1. Place a substrate on the base of the reaction chamber (105) of the vapor deposition process, and load the inorganic metal precursor and organic ligand into precursor bottle one (101) and precursor bottle two (102) respectively; open nitrogen pressure reducing valve one (201) to 0.55MPa and nitrogen pressure reducing valve two (202) to 0.14MPa as power gas and carrier gas; turn on vacuum pump (302) to evacuate the system to vacuum and heat precursor bottle one (101) and precursor bottle two (102), reaction chamber, gas inlet pipe and gas outlet pipe; After opening the precursor manual valve one (103) and precursor manual valve two (104), the following cycle is entered: opening solenoid valve one (203) to allow the inorganic metal precursor to enter the reaction chamber and be deposited, closing solenoid valve one (203) and opening shut-off valve (301) to purge excess gas; opening solenoid valve two (204) to allow the organic ligand to enter the reaction chamber and be deposited, closing solenoid valve two (204) and opening shut-off valve (301) to purge excess gas; after multiple cycles, a positive photoresist film is deposited on the substrate surface.

[0008] S2. The positive photoresist film deposited on the substrate surface is patterned and exposed using an ultraviolet lithography machine or an electron beam.

[0009] S3. Place the patterned film on top of the heating plate and heat for 1 to 5 minutes to erase the pattern, then repeat the patterning exposure on the film.

[0010] S4. After exposing the photoresist film sample to the developer for 30 seconds, quickly immerse the sample in ultrapure water or isopropanol for 10 seconds, and then use a high-pressure nitrogen gun to dry the sample surface to form a pattern.

[0011] Preferably, the molar ratio of the inorganic metal precursor to the organic ligand is 1:1 to 5.

[0012] More preferably, the molar ratio of the inorganic metal precursor to the organic ligand is 1:1, 1:3, or 1:5.

[0013] Preferably, the inorganic metal precursor is selected from at least one of tetra(dimethylamino)hafnium (TDMAHf) and tetra(dimethylamino)tin; the organic ligand is selected from at least one of maleic anhydride (MAH) and maleic acid.

[0014] Preferably, in step S1, the system is evacuated to a vacuum and the precursor bottle one (101) is heated to 75-85°C, the precursor bottle two (102) to 85-95°C, the reaction chamber (105) to 115-125°C, the inlet pipe to 115-125°C, and the outlet pipe to 95-105°C.

[0015] Preferably, in step S2, the light source wavelength of the ultraviolet lithography machine is 254nm and the exposure dose is 600MJ.

[0016] Preferably, in step S2, the electron beam current is 100 pA and the exposure dose is 400 μC.

[0017] Preferably, in step S3, the heating temperature for erasing the pattern on the heated positive photoresist film is 50–150°C.

[0018] Preferably, in step S4, the developing solution is an oxalic acid solution with a mass fraction of 0.01%.

[0019] Due to the application of the above technical solution, the present invention has the following beneficial effects compared with the prior art:

[0020] 1. The erasable organic-inorganic hybrid patterned thin film prepared by molecular layer deposition of the present invention is formed by alternating introduction of inorganic metal precursors and organic ligands on the surface of a semiconductor substrate through self-assembly. This method makes full use of the self-limiting reaction characteristics of molecular layer deposition (MLD) technology to achieve precise control of film thickness and composition ratio. By optimizing the precursor pulse time and cycle number, the sensitivity and etching resistance of the film can be significantly improved.

[0021] 2. The erasable organic-inorganic hybrid patterned thin film prepared by molecular layer deposition of the present invention has precise controllable film thickness and extremely high surface flatness, with a surface morphology (RMS) roughness of only 0.12 nanometers. It does not require the complex step of baking (PEB) after exposure. Electron beam exposure can achieve high-resolution patterns with a period of 100 nm and a linewidth of 50 nm. This film can be patterned and can be erased by heating. The present invention can be patterned after exposure and the heating is reversible, which has broad application prospects and research and development value. Attached Figure Description

[0022] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, some of the drawings in the following description are some embodiments of the present invention. For those skilled in the art, other drawings can be made based on these drawings without creative effort.

[0023] Figure 1 is a schematic diagram of the molecular layer deposition apparatus of Embodiment 1 of the present invention;

[0024] Figure 2 is a schematic diagram of the molecular layer deposition mechanism of TDMAHf and MAH in Example 1 of the present invention;

[0025] Figure 3 shows the thin film obtained after 100 cycles in Example 1 of the present invention;

[0026] Figure 4 is an AFM characterization diagram of the thin film obtained after 100 cycles in Example 1 of the present invention;

[0027] Figure 5 is a light mirror image of the thin film exposure patterning in Embodiment 1 of the present invention;

[0028] Figure 6 is a microscopic image of the patterning and erasing / rewriting process of TDMAHf:MAH = 1:5 in Embodiment 1 of the present invention.

[0029] Figure 7 is a microscopic image of the patterning and erasing / rewriting process of TDMAHf:MAH = 1:3 in Embodiment 2 of the present invention.

[0030] Figure 8 is a microscopic image of the patterning and erasing / rewriting process of TDMAHf:MAH = 1:1 in Embodiment 3 of the present invention.

[0031] Figure 9 is an optical microscope image of DUV exposure and development in Embodiment 4 of the present invention;

[0032] Figure 10 shows the infrared spectra of the photoresist film before and after exposure in Embodiment 4 of the present invention.

[0033] Figure 11 is a schematic diagram of the exposure mechanism in Embodiment 4 of the present invention;

[0034] Figure 12 is a SEM image of electron beam exposure and development in Embodiment 5 of the present invention;

[0035] In Figure 1: 101-Precursor bottle one; 102-Precursor bottle two; 103-Precursor manual valve one; 104-Precursor manual valve two; 105-Reaction chamber; 201-Nitrogen pressure reducing valve one; 202-Nitrogen pressure reducing valve two; 203-Solenoid valve one; 204-Solenoid valve two; 301-Stop valve; 302-Vacuum pump. Detailed Implementation

[0036] To provide a clearer understanding of the technical features, objectives, and effects of this invention, specific implementation schemes are now described in detail.

[0037] The present invention will be further described below with reference to embodiments, but the present invention is not limited to the following embodiments. The implementation conditions used in the embodiments can be further adjusted according to different requirements of specific use, and the implementation conditions not specified are conventional conditions in the industry. The technical features involved in the various embodiments of the present invention can be combined with each other as long as they do not conflict with each other.

[0038] Example 1

[0039] Referring to Figures 1-6, this embodiment provides an erasable organic-inorganic hybrid patterned thin film prepared by molecular layer deposition. The molecular layer deposition preparation includes the following steps:

[0040] S1. Place a substrate on the base of the reaction chamber 105 of the vapor deposition process. Load the TDMAHf precursor and MAH organic ligand into precursor bottle 101 and precursor bottle 202, respectively; the molar ratio of the inorganic metal precursor to the organic ligand is 1:5. Open nitrogen pressure reducing valve 101 to 0.55 MPa and nitrogen pressure reducing valve 202 to 0.14 MPa, using them as the power gas and carrier gas, respectively. Turn on vacuum pump 302 to evacuate the system to a vacuum and heat precursor bottle 101 to 80°C, precursor bottle 202 to 90°C, reaction chamber 105 to 120°C, inlet pipe to 120°C, and outlet pipe to 100°C. Open precursor manual valve 103 and precursor manual valve 203. 4. The following cycle is then performed: Solenoid valve 203 is opened to allow the inorganic metal precursor to enter the reaction chamber and deposit. Solenoid valve 203 is closed and shut-off valve 301 is opened to purge excess gas. Solenoid valve 204 is opened to allow the organic ligand to enter the reaction chamber and deposit. Solenoid valve 204 is closed and shut-off valve 301 is opened to purge excess gas. After 100 cycles, a positive photoresist film is deposited on the substrate surface. The specific deposition sequence is: MAH dose 1.0s / dwell 30s / exhaust 30s / TDMAHf dose 0.2s / dwell 20s / exhaust 20s. The deposition mechanism is shown in Figure 2. After deposition, the film is shown in Figure 3. The AFM characterization of the film is shown in Figure 4.

[0041] S2. A positive photoresist film with a thickness of 45 nm deposited on the substrate surface is subjected to ultraviolet lithography and controlled to adhere tightly to the photomask. The wavelength of the light source of the ultraviolet lithography machine is 254 nm. After setting the exposure dose to 600 mJ, the sample is patterned and exposed. The optical microscope image after exposure is shown in Figure 5.

[0042] S3. Place the patterned film on a heating plate and heat it at 50°C for 1 minute until the pattern disappears. Then, reposition the film and attach it to the sample stage of the deep ultraviolet lithography machine, ensuring it adheres tightly to the mask. Set the exposure dose to 600 mJ and expose the sample with a new pattern. The optical microscope image of this process is shown in Figure 6.

[0043] S4. After exposing the photoresist film sample to a 0.01% oxalic acid solution for 30 seconds, quickly immerse the sample in ultrapure water or isopropanol for 10 seconds, and then use a high-pressure nitrogen gun to dry the sample surface to form a pattern.

[0044] Example 2

[0045] Referring to Figure 7, this embodiment provides an erasable organic-inorganic hybrid patterned thin film prepared by molecular layer deposition, wherein the molecular layer deposition preparation includes the following steps:

[0046] S1. Place the substrate on the base of the reaction chamber of the vapor deposition process. Load the TDMAHf precursor and MAH organic ligand into precursor bottle one and precursor bottle two, respectively; the molar ratio of the inorganic metal precursor to the organic ligand is 1:3. Open nitrogen pressure reducing valve one to 0.55 MPa and nitrogen pressure reducing valve two to 0.14 MPa, using them as the power gas and carrier gas, respectively. Turn on the vacuum pump to evacuate the system to a vacuum and heat precursor bottle one to 80°C, precursor bottle two to 90°C, the reaction chamber to 120°C, the inlet pipe to 120°C, and the outlet pipe to 100°C; open the front... After manual valve 1 for the precursor and manual valve 2 for the precursor, the following cycle begins: Solenoid valve 1 is opened to allow the inorganic metal precursor to enter the reaction chamber and deposit; solenoid valve 1 is closed and the shut-off valve is opened to purge excess gas. Solenoid valve 2 is opened to allow the organic ligand to enter the reaction chamber and deposit; solenoid valve 2 is closed and the shut-off valve is opened to purge excess gas. After 100 cycles, a positive photoresist film is deposited on the substrate surface. The specific deposition sequence is: MAH dose 0.6s / dwell 30s / exhaust 30s / TDMAHf dose 0.2s / dwell 20s / exhaust 20s.

[0047] S2. A positive photoresist film with a thickness of 42nm deposited on the substrate surface is subjected to ultraviolet lithography and controlled to adhere tightly to the mask. The wavelength of the light source of the ultraviolet lithography machine is 254nm. After setting the exposure dose to 600mJ, the sample is patterned and exposed.

[0048] S3. The patterned film is placed on a heating plate and heated at 100°C for 1 min and 150°C for 3 min until the pattern disappears. The film is then repositioned and adsorbed onto the sample stage of the deep ultraviolet lithography machine, and its adhesion to the mask is controlled. The exposure dose is set to 600 mJ and the sample is then exposed to a new pattern. The optical microscope image of this process is shown in Figure 7.

[0049] S4. After exposing the photoresist film sample to a 0.01% oxalic acid solution for 30 seconds, quickly immerse the sample in ultrapure water or isopropanol for 10 seconds, and then use a high-pressure nitrogen gun to dry the sample surface to form a pattern.

[0050] Example 3

[0051] Referring to Figure 8, this embodiment provides an erasable organic-inorganic hybrid patterned thin film prepared by molecular layer deposition, wherein the molecular layer deposition preparation includes the following steps:

[0052] S1. Place the substrate on the base of the reaction chamber of the vapor deposition process. Load the TDMAHf precursor and MAH organic ligand into precursor bottle one and precursor bottle two, respectively; the molar ratio of the inorganic metal precursor to the organic ligand is 1:1. Open nitrogen pressure reducing valve one to 0.55 MPa and nitrogen pressure reducing valve two to 0.14 MPa, using them as the power gas and carrier gas, respectively. Turn on the vacuum pump to evacuate the system to a vacuum and heat precursor bottle one to 80°C, precursor bottle two to 90°C, the reaction chamber to 120°C, the inlet pipe to 120°C, and the outlet pipe to 100°C; open the front... After manual valve 1 for the precursor and manual valve 2 for the precursor, the following cycle begins: Solenoid valve 1 is opened to allow the inorganic metal precursor to enter the reaction chamber and deposit; solenoid valve 1 is closed and the shut-off valve is opened to purge excess gas. Solenoid valve 2 is opened to allow the organic ligand to enter the reaction chamber and deposit; solenoid valve 2 is closed and the shut-off valve is opened to purge excess gas. After 100 cycles, a positive photoresist film is deposited on the substrate surface. The specific deposition sequence is: MAH dose 0.2s / dwell 30s / exhaust 30s / TDMAHf dose 0.2s / dwell 20s / exhaust 20s.

[0053] S2. A positive photoresist film with a thickness of 40 nm deposited on the substrate surface is subjected to ultraviolet lithography and controlled to adhere tightly to the mask. The light source wavelength of the ultraviolet lithography machine is 254 nm. After setting the exposure dose to 600 mJ, the sample is patterned and exposed.

[0054] S3. Place the patterned film on a heating plate and heat it at 150°C for 5 minutes until the pattern disappears. Then, place the film back on the deep ultraviolet lithography machine sample stage and control it to adhere tightly to the mask. After setting the exposure dose to 600mJ, expose the sample for new patterning. The optical microscope image of this process is shown in Figure 8.

[0055] S4. After exposing the photoresist film sample to a 0.01% oxalic acid solution for 30 seconds, quickly immerse the sample in ultrapure water or isopropanol for 10 seconds, and then use a high-pressure nitrogen gun to dry the sample surface to form a pattern.

[0056] Example 4

[0057] Referring to Figures 9-11, this embodiment provides an erasable organic-inorganic hybrid patterned thin film prepared by molecular layer deposition. The molecular layer deposition preparation includes the following steps:

[0058] S1. Place the substrate on the base of the reaction chamber of the vapor deposition process. Load the TDMAHf precursor and MAH organic ligand into precursor bottle one and precursor bottle two, respectively; the molar ratio of the inorganic metal precursor to the organic ligand is 1:5. Open nitrogen pressure reducing valve one to 0.55 MPa and nitrogen pressure reducing valve two to 0.14 MPa, using them as the power gas and carrier gas, respectively. Turn on the vacuum pump to evacuate the system to a vacuum and heat precursor bottle one to 80°C, precursor bottle two to 90°C, and the reaction chamber to... 120℃, inlet pipe to 120℃, outlet pipe to 100℃; after opening precursor manual valve one and precursor manual valve two, the following cycle begins: open solenoid valve one to allow the inorganic metal precursor to enter the reaction chamber and deposit, close solenoid valve one and open the shut-off valve to purge excess gas; open solenoid valve two to allow the organic ligand to enter the reaction chamber and deposit, close solenoid valve two and open the shut-off valve to purge excess gas; after 100 cycles, a positive photoresist film is deposited on the substrate surface.

[0059] S2. A positive photoresist film with a thickness of 40 nm deposited on the substrate surface is subjected to ultraviolet lithography and controlled to adhere tightly to the mask. The light source wavelength of the ultraviolet lithography machine is 254 nm. After setting the exposure dose to 600 mJ, the sample is patterned and exposed.

[0060] S3. Place the patterned film on a heating plate and heat it at 50°C for 1 minute until the pattern disappears.

[0061] S4. After exposing the photoresist film sample, immerse it in a 0.01% oxalic acid solution for 30 seconds, then quickly immerse it in ultrapure water or isopropanol for 10 seconds. Finally, use a high-pressure nitrogen gun to dry the sample surface to form a pattern. Observe the sample after exposure and development using an optical microscope, as shown in Figure 9. The FTIR images of the sample before and after exposure in this example are shown in Figure 10, and the exposure mechanism is shown in Figure 11.

[0062] Example 5

[0063] Referring to Figure 12, this embodiment provides an erasable organic-inorganic hybrid patterned thin film prepared by molecular layer deposition. The molecular layer deposition preparation includes the following steps:

[0064] S1. Place the substrate on the base of the reaction chamber of the vapor deposition process. Load the TDMAHf precursor and MAH organic ligand into precursor bottle one and precursor bottle two, respectively; the molar ratio of the inorganic metal precursor to the organic ligand is 1:5. Open nitrogen pressure reducing valve one to 0.55 MPa and nitrogen pressure reducing valve two to 0.14 MPa, using them as the power gas and carrier gas, respectively. Turn on the vacuum pump to evacuate the system to a vacuum and heat precursor bottle one to 80°C, precursor bottle two to 90°C, and the reaction chamber to... 120℃, inlet pipe to 120℃, outlet pipe to 100℃; after opening precursor manual valve one and precursor manual valve two, the following cycle begins: open solenoid valve one to allow the inorganic metal precursor to enter the reaction chamber and deposit, close solenoid valve one and open the shut-off valve to purge excess gas; open solenoid valve two to allow the organic ligand to enter the reaction chamber and deposit, close solenoid valve two and open the shut-off valve to purge excess gas; after 100 cycles, a positive photoresist film is deposited on the substrate surface.

[0065] S2. Expose the 45nm thick positive photoresist film deposited on the substrate surface with an electron beam, setting the exposure dose to 400μC and the beam current to 50pA to pattern the sample.

[0066] S3. Place the patterned film on a heating plate and heat it at 50°C for 1 minute until the pattern disappears.

[0067] S4. After exposing the photoresist film sample to 0.01% oxalic acid solution for 30 seconds, quickly immerse the sample in ultrapure water or isopropanol for 10 seconds, and then use a high-pressure nitrogen gun to dry the sample surface to form a pattern. Observe the exposed and developed sample with a scanning electron microscope at a resolution of at least 50 nm, as shown in Figure 12.

[0068] Comparative Example 1

[0069] This comparative example is a thin film with a thickness of 40 nm deposited by vapor deposition with a ratio of tetramethylamino to methacrylic acid of 1:3. After exposure at 254 nm and 600 mJ, no pattern was observed under a light microscope, and the exposure could not be reversed by heating at 150 °C for 5 minutes.

[0070] Comparative Example 2

[0071] This comparative example is a thin film with a thickness of 40 nm deposited by vapor deposition with a ratio of tetramethylamino to isobutyric acid of 1:3. After exposure at 254 nm and 600 mJ, no pattern was observed under a light microscope, and the exposure could not be reversed by heating at 150 °C for 5 minutes.

[0072] In summary, the erasable organic-inorganic hybrid patterned thin film prepared by molecular layer deposition of the present invention forms an erasable patterned organic-inorganic hybrid thin film on the surface of a semiconductor substrate by alternating the introduction of inorganic metal precursors and organic ligands. This method fully utilizes the self-limiting reaction characteristics of molecular layer deposition (MLD) technology to achieve precise control of film thickness and composition ratio. By optimizing the precursor pulse time and cycle number, the sensitivity and etching resistance of the film can be significantly improved. The erasable organic-inorganic hybrid patterned thin film prepared by molecular layer deposition of the present invention has precisely controllable film thickness and extremely high surface flatness, with a surface morphology (RMS) roughness of only 0.12 nm. It does not require the complex step of baking (PEB) after exposure. Electron beam exposure can achieve high-resolution patterns with a period of 100 nm and a linewidth of 50 nm. This film can be patterned and can be erased by heating. The present invention can be patterned after exposure and the heating is reversible, which has broad application prospects and research and development value.

[0073] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this invention patent should be determined by the appended claims.

Claims

1. A molecular layer deposition prepared erasable organic-inorganic hybrid patterned thin film, characterized by, The molecular layer deposition preparation includes the following steps: S1. Place a substrate on the base of the reaction chamber (105) of the vapor deposition process, and load the inorganic metal precursor and organic ligand into precursor bottle one (101) and precursor bottle two (102) respectively; open nitrogen pressure reducing valve one (201) to 0.55MPa and nitrogen pressure reducing valve two (202) to 0.14MPa as power gas and carrier gas; turn on vacuum pump (302) to evacuate the system to vacuum and heat precursor bottle one (101) and precursor bottle two (102), reaction chamber, gas inlet pipe and gas outlet pipe; After opening the precursor manual valve one (103) and precursor manual valve two (104), the following cycle is entered: opening solenoid valve one (203) to allow the inorganic metal precursor to enter the reaction chamber and be deposited, closing solenoid valve one (203) and opening shut-off valve (301) to purge excess gas; opening solenoid valve two (204) to allow the organic ligand to enter the reaction chamber and be deposited, closing solenoid valve two (204) and opening shut-off valve (301) to purge excess gas; after multiple cycles, a positive photoresist film is deposited on the substrate surface. S2. The positive photoresist film deposited on the substrate surface is patterned and exposed using an ultraviolet lithography machine or an electron beam. S3. Place the patterned film on top of the heating plate and heat for 1 to 5 minutes to erase the pattern, then repeat the patterning exposure on the film. S4. After exposing the photoresist film sample to the developer for 30 seconds, quickly immerse the sample in ultrapure water or isopropanol for 10 seconds, and then use a high-pressure nitrogen gun to dry the sample surface to form a pattern. The inorganic metal precursor is selected from at least one of tetra(dimethylamino)hafnium and tetra(dimethylamino)tin; the organic ligand is selected from at least one of maleic anhydride and maleic acid.

2. The erasable organic-inorganic hybrid patterned thin film prepared by molecular layer deposition as described in claim 1, characterized in that, In step S1, the system is evacuated to a vacuum and the precursor bottle one (101) is heated to 75-85°C, the precursor bottle two (102) to 85-95°C, the reaction chamber (105) to 115-125°C, the inlet pipe to 115-125°C, and the outlet pipe to 95-105°C.

3. The erasable organic-inorganic hybrid patterned thin film prepared by molecular layer deposition as described in claim 1, characterized in that, In step S2, the light source wavelength of the ultraviolet lithography machine is 254nm, and the exposure dose is 600MJ.

4. The erasable organic-inorganic hybrid patterned thin film prepared by molecular layer deposition as described in claim 1, characterized in that, In step S2, the electron beam current is 100 pA and the exposure dose is 400 μC.

5. The erasable organic-inorganic hybrid patterned thin film prepared by molecular layer deposition as described in claim 1, characterized in that, In step S3, the heating temperature for erasing the pattern on the heated positive photoresist film is 50–150°C.

6. The erasable organic-inorganic hybrid patterned thin film prepared by molecular layer deposition as described in claim 1, characterized in that, In step S4, the developing solution is an oxalic acid solution with a mass fraction of 0.01%.

7. The erasable organic-inorganic hybrid patterned thin film prepared by molecular layer deposition as described in claim 1, characterized in that, The molar ratio of the inorganic metal precursor to the organic ligand is 1:1 to 5.