Intracranial thrombus aspiration catheter and preparation method therefor

By designing a multi-layer structure and optimizing the coating material, the problems of adhesion, hydrophilicity, flexibility, and anti-collapse of existing intracranial thrombus aspiration catheters in complex vascular environments have been solved, improving the stability and aspiration efficiency of the catheter and ensuring the safety and effectiveness of the treatment.

WO2026237460A1PCT designated stage Publication Date: 2026-11-19SICHUAN MEDACT TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2026/077836
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-13
Filing Date
2026-02-09
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing intracranial thrombus aspiration catheters suffer from insufficient coating adhesion, poor surface hydrophilicity, inadequate flexibility and resistance to kinking, and insufficient resistance to collapse in complex vascular environments, affecting treatment efficacy and safety.

Method used

The catheter employs a multi-layered structural design, including a PTFE liner, a stainless steel or nickel-titanium alloy coil, a stainless steel wire braided layer, a segmented polyurethane plastic layer, and a radiopaque ring. It is combined with a glycerol polyacrylate, polyurethane, or polyethylene glycol coating and fabricated through processes such as co-extrusion and laser welding to optimize coating performance.

Benefits of technology

It significantly improves the coating adhesion and surface hydrophilicity of the catheter, enhances the catheter's flexibility and kinking resistance, ensures stability and aspiration efficiency in complex blood vessels, and reduces thrombus adhesion and operational risks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2026077836_19112026_PF_FP_ABST
    Figure CN2026077836_19112026_PF_FP_ABST
Patent Text Reader

Abstract

Provided are an intracranial thrombus aspiration catheter and a preparation method therefor. The catheter comprises a PTFE liner, a reinforcing layer, a segmented outer plastic layer, a platinum-iridium alloy marker band, and a coating. The reinforcing layer comprises a coil layer and a woven layer. The preparation method comprises PTFE liner extrusion, coil winding, woven layer covering, segmented plastic layer formation, marker band embedment and fixation, and coating treatment and surface functionalization. By optimizing the formulation and process of the coating, the adhesion of the coating is significantly improved to prevent detachment, and the surface hydrophilicity is enhanced to reduce thrombus adhesion, thereby improving hemocompatibility and operational performance. In addition, the multilayer structural design improves the flexibility, kink resistance, and collapse resistance of the catheter, ensuring the stability and effectiveness of the catheter in complex vascular environments.
Need to check novelty before this filing date? Find Prior Art

Description

A catheter for intracranial thrombus aspiration and its preparation method Technical Field

[0001] This invention relates to the field of medical device technology, and in particular to an intracranial thrombus aspiration catheter and its preparation method. Background Technology

[0002] Intracranial thrombus aspiration catheters are key medical devices for treating acute ischemic stroke. Acute ischemic stroke is caused by thrombus formation or embolism in large intracranial blood vessels (such as the internal carotid artery, middle cerebral artery, basilar artery, and vertebral artery), leading to cerebral ischemia, which can cause permanent brain damage or even death in severe cases. Timely restoration of blood flow is crucial for treatment, and intracranial thrombus aspiration catheters, which remove thrombi through mechanical aspiration, have become an important treatment method.

[0003] Although existing intracranial thrombus aspiration catheters have achieved certain successes in clinical applications, several technical bottlenecks and shortcomings still limit their further application and development. First, the coating adhesion of existing catheters is insufficient, making them prone to detachment in complex vascular environments. This not only affects catheter performance but may also lead to complications such as residual thrombus or vascular damage. Second, the poor hydrophilicity of the catheter surface makes it difficult to effectively reduce thrombus adhesion and improve blood compatibility, leading to increased thrombus adhesion, affecting aspiration efficiency, and thus reducing treatment success rates. Furthermore, the complex structure of intracranial blood vessels and the insufficient flexibility and anti-kinking properties of existing catheters make it difficult to ensure smooth passage through the blood vessels and reach the target location, potentially causing the catheter to become stuck or kinked within the vessel, affecting treatment outcomes. Finally, during aspiration, the catheter needs to withstand a certain negative pressure; the insufficient anti-collapse ability of existing catheters may lead to catheter deformation or blockage, reducing aspiration efficiency and increasing patient discomfort and treatment risks.

[0004] While some improvements in existing technologies have addressed the aforementioned problems to some extent, they still have significant limitations. For example, some coating technologies, although improving adhesion, often sacrifice hydrophilicity or other properties, leading to increased thrombus adhesion and negatively impacting the catheter's effectiveness. Furthermore, existing catheters often use single materials or simple composite materials, making it difficult to simultaneously meet the comprehensive requirements of flexibility, kink resistance, and collapse resistance. This single or simple material combination limits the catheter's performance in complex vascular environments. Moreover, while some improvements enhance catheter performance, their complex processes and high costs hinder large-scale production and clinical application, making it difficult to widely promote these improvements in real-world medical settings and limiting their application scope and popularity.

[0005] Chinese patent application publication number CN118490306A discloses a thrombus aspiration catheter and an interventional medical device, including a catheter body, a thrombus aspiration channel, and a drug delivery channel. The thrombus aspiration channel extends from the distal end to the proximal end, and the drug delivery channel extends from the proximal end to the distal end, each having an aspiration inlet, a drug outlet, an aspiration outlet, and a drug inlet. Although this technology achieves the dual functions of thrombus aspiration and drug delivery, it does not solve the problems of insufficient coating adhesion and poor surface hydrophilicity, which limits the catheter's performance in complex vascular environments and may affect aspiration efficiency and blood compatibility.

[0006] Chinese patent application publication number CN117731363A discloses an embolization and thrombus aspiration catheter, including a catheter, a Y-type hemostatic valve, and an embolization and thrombus aspiration device. The embolization and thrombus aspiration device includes an aspiration element, a support element, and a limiting and locking element, capable of breaking up and softening thrombi blocking the catheter without requiring catheter retraction for flushing. While this technology solves the problem of thrombus blockage within the catheter, it does not address improvements in the catheter's flexibility, kink resistance, and collapse resistance, nor does it optimize coating performance; therefore, its overall performance in complex vascular environments still needs improvement. Summary of the Invention

[0007] To address the shortcomings of existing technologies, this invention proposes an improved intracranial thrombus aspiration catheter and its preparation method, aiming to solve problems such as insufficient coating adhesion, poor surface hydrophilicity, insufficient flexibility and kinking resistance, and insufficient anti-collapse ability in existing technologies.

[0008] To achieve the above-mentioned objectives, the present invention adopts the following technical solution:

[0009] An intracranial thrombus aspiration catheter comprising a multi-layered structure from the inside out:

[0010] (a) PTFE liner: Located at the innermost layer of the catheter, it is made of polytetrafluoroethylene (PTFE) material and is used to reduce thrombus adhesion and provide a smooth lumen;

[0011] (b) Coil: Located outside the PTFE liner, it is made of stainless steel or nickel-titanium alloy springs, providing resistance to collapse;

[0012] (c) Weaving: A mesh structure woven from stainless steel wire is partially covered on the outside of the coil to improve resistance to kinking;

[0013] (d) Plastic layer: segmented design, with high-hardness polyurethane at the near end and gradually transitioning to low-hardness polyurethane at the far end, achieving the hardness gradient through co-extrusion or segmented injection molding processes.

[0014] (e) Imaging ring: made of platinum-iridium alloy and embedded in the catheter;

[0015] (f) Coating: Located on the outermost layer of a portion of the conduit, comprising at least one of glyceryl polyacrylate, polyurethane or polyethylene glycol as the base material.

[0016] Furthermore, a method for preparing an intracranial thrombus aspiration catheter is as follows:

[0017] Step 1: Prepare PTFE liner using an extruder to obtain PTFE liner;

[0018] Step 2: Wind nickel-titanium alloy wire around the outer surface of the PTFE inner liner to obtain a coil;

[0019] Step 3: Use a braiding machine to braid stainless steel wire into a mesh, partially cover the coils and heat them to obtain the braid;

[0020] Step 4: Coat the high-hardness section at the near end with polyurethane, and switch to soft polyurethane at the low-hardness section at the far end. The hardness is continuously reduced through the gradual transition zone to obtain the plastic layer.

[0021] Step 5: Embed a platinum-iridium alloy radiopaque ring in the middle section of the catheter and fix it using pulsed laser spot welding;

[0022] Step 6: Dissolve glycerol polyacrylate in acetone, add vinyltrimethoxysilane, stir and filter to obtain the inner layer solution; add the base material and glycidyl ether compound to acetone, add crosslinking agent and photoinitiator, stir and filter to obtain the surface layer solution; coat part of the catheter surface with the inner layer solution and dry it, then coat it with the surface layer solution and cure it with ultraviolet light to obtain the intracranial thrombus aspiration catheter.

[0023] Preferably, the method for preparing the intracranial thrombus aspiration catheter is as follows:

[0024] Step 1, PTFE liner: The PTFE liner is prepared using an extruder at an extrusion temperature of 380-400℃ and an inner diameter of 0.05-0.1mm to obtain the PTFE liner;

[0025] Step 2, Coil: Wind nickel-titanium alloy wire onto the outer surface of the PTFE inner liner using a coiling machine. The diameter of the nickel-titanium alloy wire is 0.05-0.1mm, the helix spacing is 0.3-0.5mm, the winding speed is 200-300rpm, and the tension is controlled at 5-10N.

[0026] Step 3, Weaving: Using a 16-axis braiding machine, stainless steel wire with a diameter of 0.02-0.04mm is woven into a mesh at a density of 60-80PPI, partially covering the coil layer, with a weaving angle of 30-45°, and heated at 280-300℃ for 5-15 seconds;

[0027] Step 4, Plastic Layer: In the high-hardness section at the near end, a twin-screw extruder is used to coat Shore D 60-70 polyurethane at an extrusion temperature of 200-220℃; in the low-hardness section at the far end, the material is switched to Shore A 80-90 soft polyurethane, and the hardness is continuously reduced through a 5-10cm gradual transition zone.

[0028] Step 5, Imaging Ring: Embed a platinum-iridium alloy imaging ring 4-6 cm from the tip of the catheter in the middle section. Fix it by spot welding with a pulsed laser. The wavelength of the pulsed laser is 1000-1100 nm and the power is 10-30 W to avoid heat damage to the plastic layer.

[0029] Step 6, Coating: Dissolve 4-7 parts by weight of glycerol polyacrylate in 30-50 parts by weight of acetone, stir at room temperature for 20-40 minutes, add 1.5-2 parts by weight of vinyltrimethoxysilane and continue stirring for 0.5-2 hours. Then filter through a 0.1-0.3 μm pore to obtain the inner layer solution. Next, add 10-20 parts by weight of the base material and 2-4 parts by weight of glycidyl ether compound to 80-100 parts by weight of acetone, stir at 40-60℃ for 30-50 minutes until completely dissolved, then add 1-2 parts by weight of crosslinking agent and 1-2 parts by weight of photoinitiator and stir for 20-40 minutes. Filter through a 0.1-0.3 μm pore to obtain the surface layer solution. Coat part of the catheter surface with the inner layer solution evenly, dry in an oven at 50-70℃, then coat with the surface layer solution and cure with ultraviolet light to obtain the intracranial thrombus aspiration catheter.

[0030] In step 6, the base material is at least one of polyurethane and polyethylene glycol.

[0031] In step 6, the glycidyl ether compound is at least one of 1,4-butanediol diglycidyl ether and trimethylolpropane triglycidyl ether.

[0032] In step 6, the crosslinking agent is at least one of trimethylolpropane trimethacrylate and pentaerythritol tetraacrylate.

[0033] In step 6, the photoinitiator is at least one of 2-hydroxy-2-methyl-1-phenylpropanone and 1-hydroxycyclohexylphenyl ketone.

[0034] In step 6, the inner layer thickness is 3-5 μm and the surface layer thickness is 5-7 μm.

[0035] In step 6, UV curing involves using 300-350nm UV light to cure for 2-5 minutes.

[0036] Glyceryl polyacrylate, as the main component of the inner coating, provides good substrate adhesion and biocompatibility.

[0037] Vinyltrimethoxysilane acts as a coupling agent to enhance the bonding force between the inner coating and the substrate, thereby improving the coating's adhesion and durability.

[0038] Polyurethane or polyethylene glycol is used as the substrate for the outer coating. Polyurethane provides good mechanical properties and flexibility, while polyethylene glycol gives the coating excellent hydrophilicity and biocompatibility.

[0039] Glycidyl ether compounds react with polyurethane or polyethylene glycol to form a network structure, enhancing the stability and hydrophilicity of the coating.

[0040] Crosslinking agents further enhance the network structure of the coating, improving its mechanical properties and durability.

[0041] Photoinitiators trigger cross-linking reactions under ultraviolet light irradiation, promoting coating curing and ensuring rapid forming and stability of the coating.

[0042] Compared with existing technologies, it has the following advantages:

[0043] 1) By optimizing the coating formulation and process, this invention significantly improves the coating adhesion of intracranial thrombus aspiration catheters, effectively preventing coating peeling and ensuring the stability and durability of the catheters during use.

[0044] 2) The intracranial thrombus aspiration catheter of the present invention has good surface hydrophilicity, which greatly reduces thrombus adhesion and improves blood compatibility and operability. Attached Figure Description

[0045] Figure 1 is a structural model diagram of the intracranial thrombus aspiration catheter of the present invention;

[0046] The multi-layered structure of the intracranial thrombus aspiration catheter, from the inside out, is as follows:

[0047] 1. PTFE liner: This is the innermost layer of the catheter, made of polytetrafluoroethylene (PTFE). Its function is to reduce the adhesion of thrombi to the inner wall of the catheter and to provide a smooth lumen for the smooth passage of thrombi during aspiration.

[0048] 2. Coil: Located on the outside of the PTFE liner, it is made of stainless steel or nickel-titanium alloy coil. The main function of this layer is to provide anti-collapse capability, ensuring that the conduit can maintain its shape and structure during use.

[0049] 3. Braiding: A mesh structure woven from stainless steel wire partially covers the outer side of the coil layer. This layer is designed to improve the catheter's resistance to kinking, making its navigation within the blood vessel smoother.

[0050] 4. Plastic layer: This is the outer layer of the catheter. It adopts a segmented design. The proximal part uses high-hardness polyurethane material to provide sufficient support, while the distal part uses low-hardness polyurethane to increase the flexibility of the catheter. The hardness gradient change from the proximal to the distal end is achieved through co-extrusion or segmented injection molding process.

[0051] 5. Contrast ring: A contrast ring made of platinum-iridium alloy is embedded in the catheter. This ring plays a contrast role in medical imaging, helping doctors monitor the position of the catheter in real time.

[0052] 6. Coating: Located on the outermost layer of part of the catheter, its base material includes at least one of glyceryl polyacrylate, polyurethane or polyethylene glycol. The function of the coating is to further improve the surface properties of the catheter, such as hydrophilicity and biocompatibility, so as to improve its performance and safety in medical operations.

[0053] This multi-layered design aims to improve the operational performance of intracranial thrombus aspiration catheters in complex vascular environments, while ensuring their stability and effectiveness. Detailed Implementation

[0054] Main source of materials:

[0055] Shore D 65 polyurethane, made in Germany, model number: D64P477, brand: Huntsman.

[0056] Shore A 85 is a flexible polyurethane material, made in Germany, model number: TPU A 85 P 4394, brand: Huntsman.

[0057] Glyceryl polyacrylate, product number: K25, Guangdong Yuemei Chemical Co., Ltd.

[0058] Polyurethane, grade: s95A, manufacturer (origin): BASF, Germany.

[0059] Polyethylene glycol, PEG-600, brand: Lotte Korea.

[0060] All other raw materials used in the embodiments and comparative examples of this invention are commercially available products.

[0061] Figure 1 shows a structural model diagram of the intracranial thrombus aspiration catheter prepared according to the embodiments and comparative examples of the present invention.

[0062] Example 1

[0063] The preparation method of an intracranial thrombus aspiration catheter is as follows:

[0064] Step 1, PTFE liner: The PTFE liner is prepared using an extruder at an extrusion temperature of 380℃ and an inner diameter of 0.08mm to obtain the PTFE liner;

[0065] Step 2, Coil: Wind nickel-titanium alloy wire onto the outer surface of the PTFE inner liner using a coiling machine. The nickel-titanium alloy wire has a diameter of 0.06 mm, a helix pitch of 0.4 mm, a winding speed of 260 rpm, and a tension control of 8 N.

[0066] Step 3, Weaving: Using a 16-axis braiding machine, 0.03mm diameter stainless steel wire is woven into a mesh at a density of 70PPI, partially covering the coil layer, with a weaving angle of 40°; heated at 300℃ for 10 seconds to fuse the weave with the coil, ensuring no delamination;

[0067] Step 4, Plastic Layer: In the high-hardness section at the near end, a twin-screw extruder is used to coat Shore D 65 polyurethane at an extrusion temperature of 210℃; in the low-hardness section at the far end, the material is switched to Shore A 85 soft polyurethane, with a continuous decrease in hardness achieved through an 8cm gradient transition zone.

[0068] Step 5, Imaging Ring: Embed a platinum-iridium alloy imaging ring (containing 90wt% platinum + 10wt% iridium) 5cm from the tip of the catheter in the middle section. Fix it by spot welding with a pulsed laser. The wavelength of the pulsed laser is 1064nm and the power is 20W to avoid heat damage to the plastic layer.

[0069] Step 6, Coating: Dissolve 6 parts by weight of glycerol polyacrylate in 40 parts by weight of acetone, stir at room temperature for 30 minutes, then add 1.8 parts by weight of vinyltrimethoxysilane and continue stirring for 1 hour. Filter through a 0.2 μm pore to obtain the inner layer solution. Next, add 15 parts by weight of polyurethane and 3 parts by weight of trimethylolpropane triglycidyl ether to 90 parts by weight of acetone, stir at 50°C for 40 minutes until completely dissolved, then add 1.5 parts by weight of pentaerythritol tetraacrylate and 1.5 parts by weight of 2-hydroxy-2-methyl-1-phenylpropanone and stir for 30 minutes. Filter through a 0.2 μm pore to obtain the surface layer solution. Coat part of the catheter surface with the inner layer solution evenly, dry in a 60°C oven to a thickness of 4 μm, then coat with the surface layer solution and cure with 310 nm ultraviolet light for 3 minutes to a thickness of 6 μm, thus obtaining the intracranial thrombus aspiration catheter.

[0070] Example 2

[0071] The preparation method of an intracranial thrombus aspiration catheter is as follows:

[0072] Step 1, PTFE liner: The PTFE liner is prepared using an extruder at an extrusion temperature of 380℃ and an inner diameter of 0.08mm to obtain the PTFE liner;

[0073] Step 2, Coil: Wind nickel-titanium alloy wire onto the outer surface of the PTFE inner liner using a coiling machine. The nickel-titanium alloy wire has a diameter of 0.06 mm, a helix pitch of 0.4 mm, a winding speed of 260 rpm, and a tension control of 8 N.

[0074] Step 3, Weaving: Using a 16-axis braiding machine, 0.03mm diameter stainless steel wire is woven into a mesh at a density of 70PPI, partially covering the coil layer, with a weaving angle of 40°; heated at 300℃ for 10 seconds to fuse the weave with the coil, ensuring no delamination;

[0075] Step 4, Plastic Layer: In the high-hardness section at the near end, a twin-screw extruder is used to coat Shore D 65 polyurethane at an extrusion temperature of 210℃; in the low-hardness section at the far end, the material is switched to Shore A 85 soft polyurethane, with a continuous decrease in hardness achieved through an 8cm gradient transition zone.

[0076] Step 5, Imaging Ring: Embed a platinum-iridium alloy imaging ring (containing 90wt% platinum + 10wt% iridium) 5cm from the tip of the catheter in the middle section. Fix it by spot welding with a pulsed laser. The wavelength of the pulsed laser is 1064nm and the power is 20W to avoid heat damage to the plastic layer.

[0077] Step 6, Coating: Dissolve 6 parts by weight of glycerol polyacrylate in 40 parts by weight of acetone, stir at room temperature for 30 minutes, then add 1.8 parts by weight of vinyltrimethoxysilane and continue stirring for 1 hour. Filter through a 0.2 μm pore to obtain the inner layer solution. Next, add 15 parts by weight of polyurethane and 3 parts by weight of 1,4-butanediol diglycidyl ether to 90 parts by weight of acetone, stir at 50°C for 40 minutes until completely dissolved, then add 1.5 parts by weight of pentaerythritol tetraacrylate and 1.5 parts by weight of 2-hydroxy-2-methyl-1-phenylpropanone and stir for 30 minutes. Filter through a 0.2 μm pore to obtain the surface layer solution. Coat part of the catheter surface with the inner layer solution evenly, dry in a 60°C oven to a thickness of 4 μm, then coat with the surface layer solution and cure with 310 nm ultraviolet light for 3 minutes to a thickness of 6 μm, thus obtaining the intracranial thrombus aspiration catheter.

[0078] Example 3

[0079] The preparation method of an intracranial thrombus aspiration catheter is as follows:

[0080] Step 1, PTFE liner: The PTFE liner is prepared using an extruder at an extrusion temperature of 380℃ and an inner diameter of 0.08mm to obtain the PTFE liner;

[0081] Step 2, Coil: Wind nickel-titanium alloy wire onto the outer surface of the PTFE inner liner using a coiling machine. The nickel-titanium alloy wire has a diameter of 0.06 mm, a helix pitch of 0.4 mm, a winding speed of 260 rpm, and a tension control of 8 N.

[0082] Step 3, Weaving: Using a 16-axis braiding machine, 0.03mm diameter stainless steel wire is woven into a mesh at a density of 70PPI, partially covering the coil layer, with a weaving angle of 40°; heated at 300℃ for 10 seconds to fuse the weave with the coil, ensuring no delamination;

[0083] Step 4, Plastic Layer: In the high-hardness section at the near end, a twin-screw extruder is used to coat Shore D 65 polyurethane at an extrusion temperature of 210℃; in the low-hardness section at the far end, the material is switched to Shore A 85 soft polyurethane, with a continuous decrease in hardness achieved through an 8cm gradient transition zone.

[0084] Step 5, Imaging Ring: Embed a platinum-iridium alloy imaging ring (containing 90wt% platinum + 10wt% iridium) 5cm from the tip of the catheter in the middle section. Fix it by spot welding with a pulsed laser. The wavelength of the pulsed laser is 1064nm and the power is 20W to avoid heat damage to the plastic layer.

[0085] Step 6, Coating: Dissolve 6 parts by weight of glycerol polyacrylate in 40 parts by weight of acetone, stir at room temperature for 30 minutes, then add 1.8 parts by weight of vinyltrimethoxysilane and continue stirring for 1 hour. Filter through a 0.2 μm pore to obtain the inner layer solution. Next, add 15 parts by weight of polyurethane and 3 parts by weight of trimethylolpropane triglycidyl ether to 90 parts by weight of acetone, stir at 50°C for 40 minutes until completely dissolved, then add 1.5 parts by weight of trimethylolpropane trimethacrylate and 1.5 parts by weight of 2-hydroxy-2-methyl-1-phenylpropanone and stir for 30 minutes. Filter through a 0.2 μm pore to obtain the surface layer solution. Coat part of the catheter surface with the inner layer solution evenly, dry in a 60°C oven to a thickness of 4 μm, then coat with the surface layer solution and cure with 310 nm ultraviolet light for 3 minutes to a thickness of 6 μm, thus obtaining the intracranial thrombus aspiration catheter.

[0086] Example 4

[0087] The preparation method of an intracranial thrombus aspiration catheter is as follows:

[0088] Step 1, PTFE liner: The PTFE liner is prepared using an extruder at an extrusion temperature of 380℃ and an inner diameter of 0.08mm to obtain the PTFE liner;

[0089] Step 2, Coil: Wind nickel-titanium alloy wire onto the outer surface of the PTFE inner liner using a coiling machine. The nickel-titanium alloy wire has a diameter of 0.06 mm, a helix pitch of 0.4 mm, a winding speed of 260 rpm, and a tension control of 8 N.

[0090] Step 3, Weaving: Using a 16-axis braiding machine, 0.03mm diameter stainless steel wire is woven into a mesh at a density of 70PPI, partially covering the coil layer, with a weaving angle of 40°; heated at 300℃ for 10 seconds to fuse the weave with the coil, ensuring no delamination;

[0091] Step 4, Plastic Layer: In the high-hardness section at the near end, a twin-screw extruder is used to coat Shore D 65 polyurethane at an extrusion temperature of 210℃; in the low-hardness section at the far end, the material is switched to Shore A 85 soft polyurethane, with a continuous decrease in hardness achieved through an 8cm gradient transition zone.

[0092] Step 5, Imaging Ring: Embed a platinum-iridium alloy imaging ring (containing 90wt% platinum + 10wt% iridium) 5cm from the tip of the catheter in the middle section. Fix it by spot welding with a pulsed laser. The wavelength of the pulsed laser is 1064nm and the power is 20W to avoid heat damage to the plastic layer.

[0093] Step 6, Coating: Dissolve 6 parts by weight of glycerol polyacrylate in 40 parts by weight of acetone, stir at room temperature for 30 minutes, then add 1.8 parts by weight of vinyltrimethoxysilane and continue stirring for 1 hour. Filter through a 0.2 μm pore to obtain the inner layer solution. Next, add 15 parts by weight of polyethylene glycol and 3 parts by weight of trimethylolpropane triglycidyl ether to 90 parts by weight of acetone, stir at 50°C for 40 minutes until completely dissolved, then add 1.5 parts by weight of pentaerythritol tetraacrylate and 1.5 parts by weight of 2-hydroxy-2-methyl-1-phenylpropanone and stir for 30 minutes. Filter through a 0.2 μm pore to obtain the surface layer solution. Coat part of the catheter surface with the inner layer solution evenly, dry in a 60°C oven to a thickness of 4 μm, then coat with the surface layer solution and cure with 310 nm ultraviolet light for 3 minutes to a thickness of 6 μm, thus obtaining the intracranial thrombus aspiration catheter.

[0094] Comparative Example 1

[0095] The preparation method of an intracranial thrombus aspiration catheter is as follows:

[0096] Step 1, PTFE liner: The PTFE liner is prepared using an extruder at an extrusion temperature of 380℃ and an inner diameter of 0.08mm to obtain the PTFE liner;

[0097] Step 2, Coil: Wind nickel-titanium alloy wire onto the outer surface of the PTFE inner liner using a coiling machine. The nickel-titanium alloy wire has a diameter of 0.06 mm, a helix pitch of 0.4 mm, a winding speed of 260 rpm, and a tension control of 8 N.

[0098] Step 3, Weaving: Using a 16-axis braiding machine, 0.03mm diameter stainless steel wire is woven into a mesh at a density of 70PPI, partially covering the coil layer, with a weaving angle of 40°; heated at 300℃ for 10 seconds to fuse the weave with the coil, ensuring no delamination;

[0099] Step 4, Plastic Layer: In the high-hardness section at the near end, a twin-screw extruder is used to coat Shore D 65 polyurethane at an extrusion temperature of 210℃; in the low-hardness section at the far end, the material is switched to Shore A 85 soft polyurethane, with a continuous decrease in hardness achieved through an 8cm gradient transition zone.

[0100] Step 5, Imaging Ring: Embed a platinum-iridium alloy imaging ring (containing 90wt% platinum + 10wt% iridium) 5cm from the tip of the catheter in the middle section. Fix it by spot welding with a pulsed laser. The wavelength of the pulsed laser is 1064nm and the power is 20W to avoid heat damage to the plastic layer.

[0101] Step 6, Coating: Dissolve 6 parts by weight of glycerol polyacrylate in 40 parts by weight of acetone, stir at room temperature for 30 minutes, then add 1.8 parts by weight of vinyltrimethoxysilane and continue stirring for 1 hour. Filter through a 0.2 μm pore to obtain the inner layer solution. Next, add 15 parts by weight of polyurethane and 3 parts by weight of 1,3-propanediol cyclosulfate to 90 parts by weight of acetone, stir at 50°C for 40 minutes until completely dissolved, then add 1.5 parts by weight of pentaerythritol tetraacrylate and 1.5 parts by weight of 2-hydroxy-2-methyl-1-phenylpropanone and stir for 30 minutes. Filter through a 0.2 μm pore to obtain the surface layer solution. Coat part of the catheter surface with the inner layer solution evenly, dry in a 60°C oven to a thickness of 4 μm, then coat with the surface layer solution and cure with 310 nm ultraviolet light for 3 minutes to a thickness of 6 μm, thus obtaining the intracranial thrombus aspiration catheter.

[0102] Comparative Example 2

[0103] The preparation method of an intracranial thrombus aspiration catheter is as follows:

[0104] Step 1, PTFE liner: The PTFE liner is prepared using an extruder at an extrusion temperature of 380℃ and an inner diameter of 0.08mm to obtain the PTFE liner;

[0105] Step 2, Coil: Wind nickel-titanium alloy wire onto the outer surface of the PTFE inner liner using a coiling machine. The nickel-titanium alloy wire has a diameter of 0.06 mm, a helix pitch of 0.4 mm, a winding speed of 260 rpm, and a tension control of 8 N.

[0106] Step 3, Weaving: Using a 16-axis braiding machine, 0.03mm diameter stainless steel wire is woven into a mesh at a density of 70PPI, partially covering the coil layer, with a weaving angle of 40°; heated at 300℃ for 10 seconds to fuse the weave with the coil, ensuring no delamination;

[0107] Step 4, Plastic Layer: In the high-hardness section at the near end, a twin-screw extruder is used to coat Shore D 65 polyurethane at an extrusion temperature of 210℃; in the low-hardness section at the far end, the material is switched to Shore A 85 soft polyurethane, with a continuous decrease in hardness achieved through an 8cm gradient transition zone.

[0108] Step 5, Imaging Ring: Embed a platinum-iridium alloy imaging ring (containing 90wt% platinum + 10wt% iridium) 5cm from the tip of the catheter in the middle section. Fix it by spot welding with a pulsed laser. The wavelength of the pulsed laser is 1064nm and the power is 20W to avoid heat damage to the plastic layer.

[0109] Step 6, Coating: Dissolve 6 parts by weight of glycerol polyacrylate in 40 parts by weight of acetone, stir at room temperature for 30 minutes, then add 1.8 parts by weight of vinyltrimethoxysilane and continue stirring for 1 hour. Filter through a 0.2 μm pore to obtain the inner layer solution. Next, add 15 parts by weight of polyurethane and 3 parts by weight of trimethylolpropane triglycidyl ether to 90 parts by weight of acetone, stir at 50°C for 40 minutes until completely dissolved, then add 1.5 parts by weight of triacrylate and 1.5 parts by weight of 2-hydroxy-2-methyl-1-phenylpropanone and stir for 30 minutes. Filter through a 0.2 μm pore to obtain the surface layer solution. Coat part of the catheter surface with the inner layer solution evenly, dry in a 60°C oven to a thickness of 4 μm, then coat with the surface layer solution and cure with 310 nm ultraviolet light for 3 minutes to a thickness of 6 μm, thus obtaining the intracranial thrombus aspiration catheter.

[0110] Test Example 1

[0111] Adhesion performance test:

[0112] The adhesion was tested using the cross-cut test method, and the specific procedures are as follows:

[0113] Intracranial thrombus aspiration catheters prepared using the various embodiments and comparative examples were used. A 6×6 intersecting grid with a spacing of 1 mm was etched onto the coating surface using a crisscross cutter. 3M adhesive tape was then smoothly applied to the etched grid surface, ensuring complete coverage of the grid area. The tape was then quickly removed, and the extent of coating detachment from the substrate was observed. The number of detached grids was graded as follows: Grade 0, Grade 1, Grade 2, Grade 3, Grade 4, and Grade 5, where Grade 0 represents no coating detachment, and Grade 5 indicates significant coating detachment. The test results are shown in Table 1.

[0114] Table 1

[0115]

[0116] The data from Test Example 1 show that the intracranial thrombus aspiration catheter prepared in Example 1 exhibits good adhesion, with a detachment grade of only 0. This advantage may be due to the use of a combination of polyurethane and trimethylolpropane triglycidyl ether in its surface solution. Polyurethane possesses excellent mechanical properties and flexibility, enabling it to form strong adhesion with the substrate, while trimethylolpropane triglycidyl ether further enhances the network structure and adhesion of the coating. In contrast, although Example 2 also used a similar material system, the choice of materials differed, resulting in slightly poorer adhesion. In Comparative Examples 1 and 2, 1,3-propanediol cyclosulfate and triacrylate were used, respectively. These substances have relatively weak adhesion-enhancing effects, leading to poor coating adhesion.

[0117] Test Example 2

[0118] Contact angle test:

[0119] A 2 μL droplet of water was added to the surface of the intracranial thrombus aspiration catheters prepared in each embodiment and comparative example using a microsyringe. Immediately upon contact with the catheter surface, a side image of the droplet was captured using a video optical contact angle tension meter (LAUDA Scientific, LSA100). Subsequently, the droplet profile was analyzed using contact angle measurement software, and the contact angle value was calculated. The contact angle is inversely proportional to the surface hydrophilicity; that is, the smaller the contact angle, the stronger the surface hydrophilicity. Relevant test data are detailed in Table 2.

[0120] Table 2

[0121]

[0122] The intracranial thrombus aspiration catheter prepared in Example 4 of Test Example 2 exhibits stronger hydrophilicity, with a contact angle of only 18°. This may be due to the polyethylene glycol used in its surface solution. Polyethylene glycol is a highly hydrophilic polymer containing numerous hydrophilic groups in its molecular chain, capable of forming hydrogen bonds with water molecules, thus significantly enhancing surface hydrophilicity. Furthermore, the relatively uniform molecular structure of polyethylene glycol allows for the formation of a stable hydrophilic coating. In addition, trimethylolpropane triglycidyl ether forms a stable network structure, further enhancing the coating's hydrophilicity. Pentaerythritol tetraacrylate contains four acrylate groups, which are more numerous and evenly distributed, enabling the formation of more hydrogen bonds with water molecules, thus significantly enhancing hydrophilicity. In contrast, trimethylolpropane trimethacrylate and triglycerides have fewer polar groups and are less evenly distributed, resulting in relatively weaker hydrophilicity. While the polyurethane used in other examples and comparative examples exhibits good adhesion, its hydrophilicity is relatively weak. The 1,3-propanediol cyclosulfate and triacrylate used in Comparative Examples 1 and 2 exhibited poor hydrophilicity, resulting in large contact angles. Therefore, Example 4 achieved excellent hydrophilicity through optimized material composition, which is of great significance for the blood compatibility and operational performance of intracranial thrombus aspiration catheters in clinical applications.

Claims

1. A method of making an intracranial thrombectomy catheter, comprising: The method is as follows: Step 1, PTFE liner: The PTFE liner is prepared using an extruder at an extrusion temperature of 380-400℃ and an inner diameter of 0.05-0.1mm to obtain the PTFE liner; Step 2, Coil: Wind nickel-titanium alloy wire onto the outer surface of the PTFE inner liner using a coiling machine. The diameter of the nickel-titanium alloy wire is 0.05-0.1mm, the helix spacing is 0.3-0.5mm, the winding speed is 200-300rpm, and the tension is controlled at 5-10N. Step 3, Weaving: Using a 16-axis braiding machine, stainless steel wire with a diameter of 0.02-0.04mm is woven into a mesh at a density of 60-80PPI, partially covering the coil layer, with a weaving angle of 30-45°, and heated at 280-300℃ for 5-15 seconds; Step 4, Plastic Layer: In the high-hardness section at the near end, a twin-screw extruder is used to coat Shore D 60-70 polyurethane at an extrusion temperature of 200-220℃; in the low-hardness section at the far end, the material is switched to Shore A 80-90 soft polyurethane, and the hardness is continuously reduced through a 5-10cm gradual transition zone. Step 5, Imaging Ring: Embed a platinum-iridium alloy imaging ring 4-6 cm from the tip of the catheter in the middle section. Fix it by spot welding with a pulsed laser. The wavelength of the pulsed laser is 1000-1100 nm and the power is 10-30 W to avoid heat damage to the plastic layer. Step 6, Coating: Dissolve 4-7 parts by weight of glycerol polyacrylate in 30-50 parts by weight of acetone, stir at room temperature for 20-40 minutes, add 1.5-2 parts by weight of vinyltrimethoxysilane and continue stirring for 0.5-2 hours. Then filter through a 0.1-0.3 μm pore to obtain the inner layer solution. Next, add 10-20 parts by weight of the base material and 2-4 parts by weight of glycidyl ether compound to 80-100 parts by weight of acetone, stir at 40-60℃ for 30-50 minutes until completely dissolved, then add 1-2 parts by weight of crosslinking agent and 1-2 parts by weight of photoinitiator and stir for 20-40 minutes. Filter through a 0.1-0.3 μm pore to obtain the surface layer solution. Coat part of the catheter surface with the inner layer solution evenly, dry in an oven at 50-70℃, then coat with the surface layer solution and cure with ultraviolet light to obtain the intracranial thrombus aspiration catheter.

2. The method of claim 1, wherein, In step 6, the base material is at least one of polyurethane and polyethylene glycol.

3. The method of claim 1, wherein, In step 6, the glycidyl ether compound is at least one of 1,4-butanediol diglycidyl ether and trimethylolpropane triglycidyl ether.

4. The method as described in claim 1, characterized in that, In step 6, the crosslinking agent is at least one of trimethylolpropane trimethacrylate and pentaerythritol tetraacrylate.

5. The method as described in claim 1, characterized in that, In step 6, the photoinitiator is at least one of 2-hydroxy-2-methyl-1-phenylpropanone and 1-hydroxycyclohexylphenyl ketone.

6. The method as described in claim 1, characterized in that, In step 6, the inner layer thickness is 3-5 μm and the surface layer thickness is 5-7 μm.

7. The method as described in claim 1, characterized in that, In step 6, UV curing involves using 300-350nm UV light to cure for 2-5 minutes.

8. A catheter for aspirating intracranial thrombi, characterized in that, It is prepared by the preparation method described in any one of claims 1-7.